Silicon wafer manufacturing method

A two-step heat treatment process for silicon wafers addresses the challenge of insufficient gettering by forming sites below the surface layer, ensuring both effective gettering and a defect-free surface through controlled oxygen diffusion and precipitation.

JP7590839B2Active Publication Date: 2024-11-27GLOBALWAFERS JAPAN
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2020156443
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-09-17
Publication Date
2024-11-27
Estimated Expiration
2040-09-17

AI Technical Summary

Technical Problem

Recent semiconductor device formation processes at lower temperatures and shorter times result in insufficient diffusion of metal impurities to gettering sites in silicon wafers, limiting the gettering effect, necessitating the formation of gettering sites directly below the surface layer while maintaining a defect-free surface layer.

Method used

A two-step heat treatment process is applied to silicon wafers, involving inward diffusion of oxygen and freezing atomic vacancies in the bulk, followed by controlled nucleation and growth of oxygen precipitates several micrometers below the surface, using specific temperature and time conditions to create gettering sites and ensure a defect-free surface layer.

Benefits of technology

The method effectively forms gettering sites several micrometers below the surface while maintaining a sufficient defect-free layer, enhancing the gettering performance of silicon wafers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007590839000003
    Figure 0007590839000003
  • Figure 0007590839000004
    Figure 0007590839000004
  • Figure 0007590839000005
    Figure 0007590839000005
Patent Text Reader

Abstract

To form a gettering site several μm directly below the surface layer while ensuring a sufficient defect-free layer on the surface layer.SOLUTION: A manufacturing method of a silicon wafer includes a first heat treatment step of inwardly diffusing oxygen on a surface layer of a silicon wafer obtained by slicing from a single crystal silicon ingot grown by a Czochralski method and freezing an atomic pore in a bulk portion of the silicon wafer, and a second heat treatment step of setting an experience time from the furnace temperature to 700°C less than two hours, performing holding at 800°C or higher and 1000°C or lower for one hour or more and ten hours or less, and then raising the temperature to 1100°C or higher and 1200°C or lower and maintaining the temperature for ten minutes or longer and four hours or shorter.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for manufacturing a silicon wafer. [Background technology]

[0002] Silicon wafers (hereafter sometimes simply referred to as wafers) used as substrates for semiconductor devices are required not only to have defect-free surfaces, but also to have mechanical strength and gettering performance, which captures metal impurities, in order to improve device quality. Gettering is a technology that actively utilizes the phenomenon in which impurities in the wafer gather in specific areas to reduce the adverse effects on the performance of the final product, and can be broadly divided into intrinsic gettering and extrinsic gettering.

[0003] Intrinsic gettering (hereinafter simply referred to as gettering) reduces the adverse effect on the performance of the final product by designing oxygen precipitates called BMD (Bulk Micro Defects) inside the wafer. BMD inside the wafer can combine with metal impurities and fix them. In order to improve the performance of gettering, it is important to control the area where BMD precipitates well. For example, Patent Document 1 proposes a method in which a wafer is subjected to rapid temperature increase and decrease (hereinafter referred to as RTP) at 1300°C or higher to leave a large amount of vacancies, which are point defects, in the bulk of the wafer (not the surface layer but the inside), and then BMDs are formed at a high density during the subsequent BMD precipitation heat treatment. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2015-204326 A Summary of the Invention [Problem to be solved by the invention]

[0005] In recent years, various heat treatments in the semiconductor device fabrication process have tended to be performed at lower temperatures and in shorter times. This shortens the diffusion distance of metal impurities that have inadvertently entered the silicon wafer. As a result, the metal impurities cannot diffuse to the depth of the gettering site where the BMD is formed, and a sufficient gettering effect cannot be obtained. Therefore, in recent years, there has been a demand for so-called proximity gettering wafers, which form gettering sites several μm beneath the surface layer while ensuring a sufficient defect-free layer in the surface layer of the silicon wafer.

[0006] In view of the above-mentioned problems, an object of the present invention is to provide a method for manufacturing a silicon wafer that contributes to forming gettering sites several μm beneath the surface layer while ensuring a sufficient defect-free layer in the surface layer. [Means for solving the problem]

[0007] In order to solve the above problems, the method for producing a silicon wafer of the present invention includes a first heat treatment step of diffusing oxygen inward into a surface layer of a silicon wafer obtained by slicing a single crystal silicon ingot grown by the Czochralski method in an oxidizing atmosphere and freezing atomic vacancies in a bulk portion of the silicon wafer, and a second heat treatment step of setting the exposure time from the furnace temperature to 700°C to be less than two hours, holding the temperature at 800°C to 1000°C for 1 hour to 10 hours, and then raising the temperature to 1100°C to 1200°C and holding the temperature for 10 minutes to 4 hours.

[0008] In this way, the method for producing a silicon wafer of the present invention forms a BMD precipitation region several μm beneath the device active layer by combining a first heat treatment step and a second heat treatment step. In the first heat treatment step, oxygen is inwardly diffused into the surface layer to increase the oxygen concentration in the surface layer region, and atomic vacancies (hereinafter, vacancies) are frozen in the wafer bulk. Then, in the second heat treatment step, oxygen precipitates are made visible in the surface layer region several μm deep.

[0009] In the second heat treatment step, the time from the furnace temperature to 700°C is set to less than two hours in order to prevent the formation of oxygen precipitates in the region 1 μm below the surface. The reason for holding the temperature at 800°C to 1000°C is that this is the main nucleation temperature for oxygen precipitates caused by vacancies. The reason for holding the temperature at 1100°C to 1200°C for 10 minutes to 2 hours is to grow the nuclei of the oxygen precipitates that have been generated, increasing the surface area of ​​the precipitates and enhancing the gettering power of metal impurities.

[0010] Furthermore, in the first heat treatment step, it is preferable to hold the temperature at 1300°C to 1350°C for 1 to 60 seconds, and then rapidly cool to 1000°C at a cooling rate faster than 50°C per second, 120°C per second or less. The oxygen concentration in the surface layer region is increased by holding the temperature at 1300°C to 1350°C for 1 to 60 seconds, and the reason for setting the cooling rate faster than 50°C per second is to prevent a decrease in concentration due to outward diffusion of the increased oxygen and vacancies. Also, the reason for setting the cooling rate to 120°C per second or less is to prevent the occurrence of slip due to thermal stress.

[0011] Furthermore, it is preferable to carry out the second heat treatment successively after the first heat treatment without removing the surface layer of the silicon wafer, in order to form a defect-free layer several μm deep from the surface of the silicon wafer and a formation region of oxygen precipitates immediately below the defect-free layer.

[0012] Furthermore, after the first heat treatment, it is preferable to remove the oxide film formed on the silicon wafer and then perform the second heat treatment in a non-oxidizing atmosphere, in order to promote outward diffusion of oxygen and ensure a defect-free region of about 2 μm.

[0013] Furthermore, it is preferable to use a defect-free silicon ingot obtained by controlling the crystal pulling speed and the temperature gradient in the crystal axis direction at the solid-liquid interface in the Czochralski method. In the first heat treatment method, void defects (defects introduced during crystal growth) remain within a region 1 μm from the surface. This problem can be avoided by using defect-free silicon that does not have void defects. Effect of the Invention

[0014] According to the present invention, it is possible to provide a method for manufacturing a silicon wafer that contributes to forming gettering sites several μm beneath the surface layer while ensuring a sufficient defect-free layer in the surface layer. [Brief description of the drawings]

[0015] [Figure 1] FIG. 1 is a cross-sectional view showing an outline of an example of an RTP apparatus used in a silicon wafer manufacturing method according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a flowchart showing the steps of the method for producing a silicon wafer according to the embodiment of the present invention. [Diagram 3] FIG. 3 is a diagram showing a sequence of heat treatments in the method for producing a silicon wafer according to the present invention. [Figure 4] FIG. 4 is a diagram showing an oxygen concentration profile in the depth direction. [Diagram 5] FIG. 5 is a graph showing the change in thickness of the denuded zone. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. However, the present invention is not limited to the embodiment described below. In addition, in each drawing, the same or corresponding elements are appropriately assigned the same reference numerals. Furthermore, it should be noted that the drawings are schematic, and the dimensional relationship of each element, the ratio of each element, etc. may differ from the actual ones. There may also be parts in which the dimensional relationship and ratio differ between the drawings.

[0017] FIG. 1 is a cross-sectional view showing an outline of an example of an RTP apparatus used in a silicon wafer manufacturing method according to an embodiment of the present invention.

[0018] As shown in FIG. 1, the RTP apparatus 10 includes a chamber (reaction tube) 20 having an atmospheric gas inlet 20a and an atmospheric gas outlet 20b, a plurality of lamps 30 spaced apart from one another in the upper portion of the chamber 20, and a wafer support 40 that supports a wafer W in a reaction space 25 within the chamber 20.

[0019] The wafer support 40 includes an annular susceptor 40a that supports the outer periphery of the wafer W, and a stage 40b that supports the susceptor 40a. The wafer support 40 also includes a rotating means that rotates the wafer W around its central axis at a predetermined speed.

[0020] The chamber 20 is made of, for example, quartz. The lamp 30 is made of, for example, a halogen lamp. The susceptor 40a is made of, for example, silicon. The stage 40b is made of, for example, quartz.

[0021] 1, RTP is performed on the wafer W by introducing the wafer W into the reaction space 25 and supporting the wafer W on the susceptor 40a of the wafer support 40. Then, an atmospheric gas, which will be described later, is introduced from the atmospheric gas inlet 20a, and the surface of the wafer W is irradiated with light from the lamps 30 while the wafer W is being rotated.

[0022] The temperature in the reaction space 25 in the RTP device 10 is controlled by measuring the average temperature at multiple points on the wafer surface in the radial direction of the lower part of the wafer W using multiple radiation thermometers 50 embedded in the stage 40b of the wafer support part 40, and controlling the multiple halogen lamps 30 (such as individually controlling the ON-OFF of each lamp and controlling the emission intensity of the emitted light) based on the measured temperatures.

[0023] Fig. 2 is a flow chart showing the steps of a method for producing a silicon wafer according to an embodiment of the present invention. As shown in Fig. 2, the method for producing a silicon wafer according to an embodiment of the present invention mainly includes a silicon wafer preparation step S1, a first heat treatment step S2, and a second heat treatment step S3.

[0024] In the silicon wafer preparation step S1, silicon wafers sliced ​​from a silicon single crystal ingot grown by the Czochralski method are prepared. The growth of a silicon single crystal ingot by the Czochralski method can be performed by a known method. Polycrystalline silicon filled in a quartz crucible is heated to form a silicon melt, a seed crystal is brought into contact with the silicon melt from above the liquid surface, and the seed crystal and the quartz crucible are pulled up while rotating, and the diameter is expanded to a desired diameter to grow a straight body portion, thereby producing a silicon single crystal ingot.

[0025] Here, in the Czochralski method, it is preferable to use a defect-free silicon ingot obtained by controlling the crystal pulling speed and the temperature gradient in the crystal axis direction at the solid-liquid interface. In the first heat treatment method in the latter stage, void defects (defects introduced during crystal growth) remain within a 1 μm region from the surface. This problem can be avoided by using defect-free silicon that does not have void defects.

[0026] The silicon single crystal ingot thus obtained is processed into silicon wafers by a well-known method. The silicon single crystal ingot is sliced ​​into wafers using an inner diameter blade or a wire saw, and then processed by processes such as chamfering the outer circumference, lapping, etching, polishing, etc. to produce silicon wafers before heat treatment.

[0027] In the first heat treatment step S2, oxygen is diffused inward into the surface layer of the silicon wafer in an oxidizing atmosphere, and atomic vacancies are frozen in the bulk of the silicon wafer. In the second heat treatment step S3, oxygen precipitates are made visible in a surface layer several μm deep. The optimal conditions for the first heat treatment step S2 and the second heat treatment step S3 will be described in detail later.

[0028] On the other hand, it is preferable to perform the second heat treatment S3 after the first heat treatment S2 without removing the surface layer of the silicon wafer. This is to create a defect-free layer several μm from the surface of the silicon wafer and an oxygen precipitate formation region immediately below the defect-free layer. In addition, it is preferable to peel off the oxide film formed on the silicon wafer after the first heat treatment S2 and then perform the second heat treatment S3 in a non-oxidizing atmosphere. This is to promote the outward diffusion of oxygen and ensure a sufficient defect-free layer.

[0029] Fig. 3 is a diagram showing a sequence of heat treatments in a method for producing a silicon wafer according to the present invention. In Fig. 3, the vertical axis T indicates temperature, and the horizontal axis t indicates time. As shown in Fig. 3, the method for producing a silicon wafer according to the present invention includes a first heat treatment step TH1 and a second heat treatment step TH2.

[0030] As shown in Fig. 3, the first heat treatment step TH1 involves heating to a temperature T1, holding the temperature for a time D1, and then rapidly cooling at a cooling rate R1. The first heat treatment step TH1 is performed in an oxidizing atmosphere using, for example, an RTP apparatus 10 as shown in Fig. 1.

[0031] The temperature T1 in the first heat treatment step TH1 is preferably, for example, 1300°C or higher and 1350°C or lower, and the time D1 is preferably 1 second or higher and 60 seconds or lower. This is to sufficiently increase the oxygen concentration in the surface region of the silicon wafer. Also, the cooling rate R1 in the first heat treatment step TH1 is preferably faster than 50°C per second and 120°C per second or lower. This is to prevent a decrease in concentration due to outward diffusion of oxygen and vacancies that have been increased in the silicon wafer by heating in an oxidizing atmosphere.

[0032] 3, the second heat treatment process TH2 includes increasing the temperature to T2, holding the temperature for a time D2, and then increasing the temperature to T3 and holding the temperature for a time D3. However, the rate of increase in temperature to T2 is set so that the experience time from the furnace temperature to T4 is shorter than the time D4.

[0033] The temperature T2 in the second heat treatment step TH2 is preferably, for example, 800°C or higher and 1000°C or lower, and the time D2 is preferably 1 hour or higher and 10 hours or lower. This temperature condition is because it is the main nucleation temperature of oxygen precipitates caused by vacancies, and is preferable for generating oxygen precipitates. The temperature T3 is preferably, for example, 1100°C or higher and 1200°C or lower, and the time D3 is preferably 10 minutes or higher and 4 hours or lower. This is to grow the nuclei of the generated oxygen precipitates, increase the surface area of ​​the precipitates, and increase the gettering power of metal impurities.

[0034] It is preferable that the temperature T4 during heating in the second heat treatment step TH2 is 700° C. and the exposure time D4 to this temperature is less than 2 hours in order to prevent the formation of oxygen precipitates in the 1 μm region immediately below the surface and to ensure a sufficiently wide defect-free layer.

[0035] [Example] Next, an example will be described in which the effects of the above-described method for producing a silicon wafer according to the present invention are verified.

[0036] (Verification experiment 1) In verification experiment 1, the relationship between silicon wafers having different oxygen concentrations and the region in which oxygen precipitates occur was examined. The silicon wafers of the example used in verification experiment 1 are as follows.

[0037] [Table 1]

[0038] The silicon wafers of Examples A to C were subjected to a first heat treatment process and a second heat treatment process. In the first heat treatment process, the wafer was held at 1350°C for 30 seconds in a 100% O2 atmosphere, and then quenched at a cooling rate of 120°C per second. After the oxide film was peeled off, the second heat treatment process was performed under conditions of a 100% Ar atmosphere, with the temperature of the furnace being raised from 600°C to 700°C for 60 minutes, and the wafer was held at 850°C for 3 hours, and then held at 1150°C for 30 minutes.

[0039] The oxygen concentration profile in the depth direction was analyzed for the silicon wafers of Examples A to C that had been subjected to the first heat treatment step and the second heat treatment step using a secondary ion mass spectrometry (SIMS). Fig. 4 is a diagram showing the oxygen concentration profile in the depth direction. For comparison, Fig. 4 also shows an example (comparative example) in which only the first heat treatment step was performed on Example B, and an example (calculation example) in which calculations were performed taking only oxygen diffusion into consideration.

[0040] As shown in Fig. 4, in the example (comparative example) where only the first heat treatment step was performed, the concentration increased in the surface layer due to the inward diffusion of oxygen. On the other hand, in the examples (Examples A to C) where the first and second heat treatment steps were performed, a peak due to oxygen precipitates was detected at a depth of 1 to 6 µm. The height of the peak of oxygen precipitates in Examples A to C depends on the oxygen concentration in the silicon wafer before the first heat treatment step was performed.

[0041] In addition, in comparison with the example (calculation example) in which calculation was performed taking into account only the diffusion of oxygen, the oxygen concentration decreases toward the surface. On the other hand, in the examples (Examples A to C) in which the first heat treatment step and the second heat treatment step were performed, a peak due to oxygen precipitates was detected at a depth of 1 to 6 μm, so the principle behind the occurrence of such a profile cannot be explained by the diffusion of oxygen alone.

[0042] Furthermore, in the examples (Examples A to C) in which the first heat treatment step and the second heat treatment step were performed, a defect-free zone (DZ) was formed from the surface to a depth of about 1 μm, and the thickness of this defect-free zone was not dependent on the oxygen concentration in the silicon wafer before the first heat treatment step.

[0043] As described above, verification experiment 1 demonstrated that the second heat treatment process is effective in forming a defect-free layer of approximately 1 μm in thickness and in forming gettering sites (GS) to a depth of 1 to 6 μm in the profile of the oxygen concentration diffused inward into the surface layer of the silicon wafer by the first heat treatment process.

[0044] (Verification experiment 2) Next, an experiment was conducted to verify the effect of the exposure time from the furnace temperature to 700°C in the second heat treatment step. The silicon wafers used in this verification experiment 2 had the same oxygen concentration of 1.2 × 10 18 / cm 3 The silicon wafers were 300 mm in diameter.

[0045] In the first heat treatment step, the wafer was held at 1350°C for 30 seconds in a 100% O2 atmosphere, and then rapidly cooled at a rate of 120°C per second, as in Verification Experiment 1. After the first heat treatment step, the oxide film was peeled off, and the second heat treatment step was continued without removing the surface layer of the silicon wafer.

[0046] In the first heat treatment step, the time for which the furnace temperature was raised from 600°C to 700°C was changed in a 100% Ar atmosphere, and the effect of this exposure time on the peak of oxygen precipitates was examined. The peak of oxygen precipitates refers to the peak in the oxygen concentration profile in the depth direction as shown in Figure 4 mentioned above. This oxygen concentration profile can be measured using a secondary ion mass spectrometry (SIMS) in the same way as in Verification Experiment 1.

[0047] In verification experiment 2, the furnace temperature was changed from 600°C to 700°C for 30, 60, 120, 180, and 240 minutes, and it was measured whether or not an oxygen precipitate peak was formed in the 1 μm region immediately below the surface for each exposure time. From the viewpoint of securing a sufficiently wide defect-free zone, a product that does not form an oxygen precipitate peak in the 1 μm region immediately below the surface was determined to be good (◯), and a product that forms an oxygen precipitate peak in the 1 μm region immediately below the surface was determined to be defective (×).

[0048] [Table 2]

[0049] As shown in the above table, the exposure time D4 during the temperature rise to 700°C in the second heat treatment step TH2 is preferably less than 2 hours, because this prevents the formation of oxygen precipitates in the 1 μm region immediately below the surface of the silicon wafer and ensures a sufficiently wide defect-free layer.

[0050] (Verification experiment 3) Next, the conditions for creating a sufficiently wide defect-free zone were examined. The silicon wafer used in this verification experiment 3 had the same oxygen concentration of 1.2 × 10 18 / cm 3 The silicon wafers were 300 mm in diameter.

[0051] In the first heat treatment step, the wafer was held at 1350°C for 30 seconds in a 100% O2 atmosphere, as in the verification experiment 1, and then rapidly cooled at a cooling rate of 120°C per second. After the oxide film was peeled off, the second heat treatment step was performed under the conditions of a 100% Ar atmosphere, with the furnace temperature increased from 600°C to 700°C for 60 minutes, and the wafer was held at 850°C for 3 hours, but the subsequent holding time at 1150°C was changed from 1 minute to 5 hours. The change in thickness of the denuded layer was examined for the silicon wafers obtained as a result. Figure 5 shows the change in thickness of the denuded layer.

[0052] As shown in FIG. 5, the thickness of the denuded zone (DZ width) increases depending on the holding time at 1150°C. This is because the longer the holding time at 1150°C, the more the outward diffusion of oxygen in the surface layer progresses. However, holding time at 1150°C for shorter than 10 minutes is not preferable because the thickness of the denuded zone is insufficient. On the other hand, holding time at 1150°C for longer than 4 hours does not show a significant change in the thickness of the denuded zone, which is not preferable from the viewpoint of efficiency. Therefore, the holding time at 1150°C is preferably 10 minutes or more and 4 hours or less.

[0053] As described above, it has been demonstrated that the method for producing a silicon wafer of the present invention can produce a so-called proximity gettering wafer having a denuded layer thickness of 1 to 2 μm and a gettering site depth of 1 to 6 μm.

[0054] Although the present invention has been described based on the embodiments with reference to the drawings, the present invention is not limited to the above-mentioned embodiments. In particular, it should be understood that the numerical ranges described in this specification can be modified or changed without departing from the technical spirit of the present invention. [Explanation of symbols]

[0055] 10 RTP device 20 Chamber 20a Atmospheric gas inlet 20b Atmospheric gas exhaust port 25 Reaction Space 30 Lamp 40 Wafer support

Claims

1. A silicon wafer having an oxygen concentration of 0.5×10 18 / cm 3 or more and 1.0×10 18 / cm 3 or less is obtained by slicing a defect-free single crystal silicon ingot grown by controlling the crystal pulling speed and the temperature gradient in the crystal axis direction at the solid-liquid interface in the Czochralski method, a first heat treatment step of inwardly diffusing oxygen into a surface layer of the silicon wafer and freezing atomic vacancies in a bulk portion of the silicon wafer in an oxidizing atmosphere; A second heat treatment step is performed in a non-oxidizing atmosphere, in which the exposure time from the furnace temperature to 700°C is less than 2 hours, and the temperature is maintained at 800°C to 1000°C for 1 hour to 10 hours, and then the temperature is increased to 1100°C to 1200°C and maintained for 10 minutes to 4 hours; wherein the second heat treatment step is performed after removing an oxide film formed on the silicon wafer after the first heat treatment step.

2. 2. The method for producing a silicon wafer according to claim 1, wherein the first heat treatment step comprises holding the wafer at 1300° C. or more and 1350° C. or less for 1 second or more and 60 seconds or less, and quenching the wafer to 1000° C. or less at a cooling rate faster than 50° C. per second and 120° C. per second or less.

Citation Information

Patent Citations

  • Method of thermally treating silicon wafer

    JP2006261632A

  • Manufacturing method of silicon single crystal wafer

    JP2008207991A

  • Manufacturing method of silicon wafer

    JP2011243923A

  • Heat treatment method for silicon wafer

    JP2013074139A

  • Silicon single crystal wafer manufacturing method and electronic device

    JP2013143504A