Filter media, elements, and methods
The filter media with a surface-loaded and deep-loaded layer configuration addresses the need for high-efficiency, low-pressure-drop filtration, achieving exceptional particle removal and extended filter life with self-cleaning capabilities.
Patent Information
- Application Number
- JP2022150470
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2016-06-17
- Filing Date
- 2022-09-21
- Publication Date
- 2024-11-27
- Estimated Expiration
- 2037-05-05
AI Technical Summary
There is a need for high-performance filters that provide high efficiency, low pressure drop, and long life to effectively remove particulate matter from fluid streams, particularly in applications such as air intake for engines and gas turbines, while minimizing maintenance and operational costs.
The development of filter media and elements comprising a surface-loaded filter layer with fine fibers, a deep-loaded filter layer, and a support layer, configured to maximize filtration efficiency and minimize pressure drop, with optional pulse-cleanability for self-cleaning.
The filter media achieves high filtration efficiency, with the ability to remove at least 99.995% of 0.4 micron particles, while maintaining low pressure drop and extending the filter's lifespan, thus reducing maintenance and operational costs.
Smart Images

Figure 0007591013000013 
Figure 0007591013000014 
Figure 0007591013000015
Abstract
Description
[Technical field]
[0001] Continuing Application Data This application claims the benefit of U.S. Provisional Patent Application No. 62 / 336,433, filed May 13, 2016, and U.S. Provisional Patent Application No. 62 / 351,401, filed June 17, 2016, the disclosures of each of which are incorporated herein by reference in their entireties. [Background technology]
[0002] Fluid streams, particularly air and gas streams, often carry particulate material. Removal of some or all of the particulate material from the fluid stream is desired. For example, intake streams to the passenger compartment of an electric vehicle, air in computer disk drives, HVAC air, circulating air in clean rooms, air to engines for vehicles or power plants, gas streams directed to gas turbines, and air streams to various combustion furnaces often contain particulate material therein. In the case of cabin air filters, it is desirable to remove particulate matter for passenger comfort and / or aesthetics. With respect to air and gas intake streams to engines, gas turbines, and combustion furnaces, it is desirable to remove particulate material because the fine particles can cause substantial damage to the internal workings of the various devices involved. In another example, manufacturing gases or exhaust gases from industrial processes or engines may contain particulate material therein. It is generally desirable to achieve substantial removal of particulate material from these streams before such gases are exhausted to the atmosphere. Summary of the Invention [Problem to be solved by the invention]
[0003] Increasingly higher efficiency filters are needed to obtain cleaner air or other gas flows. Lower pressures are desirable to reduce the restriction on gas (e.g., air) flow caused by high efficiency filters. Longer life is also desirable to reduce maintenance and filter costs that are often challenges with high efficiency filters. Thus, there is a continuing need for high performance filters, i.e., filters that are highly efficient, have low pressure drop, and have long life. [Means for solving the problem]
[0004] The present disclosure provides filter media and filter elements, particularly for gas (eg, air) filtration applications.
[0005] In one embodiment, a gas filter media (e.g., air filter media) is provided that includes a surface-loaded filter layer that includes fine fibers having an average diameter of less than 1 micron, a depth-loaded layer, and a support layer. In use, the layers are configured and arranged for placement in a gas stream with the surface-loaded filter layer being the most upstream layer. That is, the layers are positioned relative to one another such that the surface-loaded filter layer is positioned as the first layer encountered by the gas (e.g., air) stream being filtered (i.e., the fine fiber filter layer is the most upstream layer). In certain embodiments, the filter media of the present disclosure are pulse washable.
[0006] In another embodiment of the present disclosure, a gas filter element (eg, an air filter element) is provided that includes a housing and a filter media as described herein.
[0007] In another embodiment of the present disclosure, a method of filtering a gas (e.g., air) is provided that includes directing the gas through a filter medium or filter element as described herein.
[0008] In certain embodiments, the depth load filter layer comprises a high efficiency glass-containing filter layer, a meltblown filter layer, or a combination thereof. The high efficiency glass-containing filter layer may comprise glass fibers and multicomponent binder fibers. The high efficiency meltblown filter layer may comprise fibers having an average diameter between 0.5 microns and 10 microns.
[0009] As used herein, "high efficiency" with respect to a filter layer of the present disclosure means being able to remove at least 55% (by number) of 0.4 micron sized DEHS particles at 4 feet per minute (ft / min or fpm) (i.e., 2 centimeters per second (cm / sec)). For example, a filtration efficiency of at least 70% at 0.4 microns is considered "high efficiency." In certain embodiments herein, high efficiency means removing at least 70%, at least 80%, at least 85%, at least 95%, at least 99.5%, at least 99.95%, or at least 99.995% of such particles at 4 ft / min (2 cm / sec).
[0010] As used herein, "high efficiency" for the composite filter media (which may or may not be corrugated) and / or filter elements (which are typically corrugated and pleated) of the present disclosure refers to an efficiency of at least F9 according to EN779:2012. Additionally, "high efficiency" filter elements (which are typically corrugated and pleated) of the present disclosure refer to an efficiency of at least E10, or at least E11, or at least E12 according to EN1822:2009.
[0011] The term "meltblown fiber" refers to fibers formed by extruding molten thermoplastic material as molten threads or filaments through multiple precise, usually circular, die capillaries into a converging high velocity gas (e.g., air) stream that attenuates the filaments of molten thermoplastic material to reduce their diameter, which may be the diameter of a microfiber. The meltblown fibers are then carried by the high velocity gas stream and deposited on a collecting surface to form a web of randomly distributed meltblown fibers. Typically, meltblown fibers are microfibers that may be continuous or discontinuous, generally have a diameter of 20 microns or less (often 10 microns), and generally self-bond when deposited on a collecting surface. The meltblown fibers used in the present invention are preferably substantially continuous in length.
[0012] The term "multicomponent fiber" refers to a fiber formed from at least two polymers that are extruded separately but spun together to form one fiber. As a specific example of a multicomponent fiber, a "bicomponent fiber" includes two polymers arranged in distinct zones that are substantially always positioned across the cross section of the bicomponent fiber and extend continuously along the length of the bicomponent fiber. The configuration of such bicomponent fibers may be, for example, a sheath / core configuration, where one polymer is surrounded by another polymer, or a side-by-side or "islands-in-the-sea" configuration. For bicomponent fibers, the polymers may be present in a 75 / 25, 50 / 50, 25 / 75 ratio or any other desired ratio. Conventional additives, such as pigments and surfactants, may be incorporated into one or both polymer streams or applied to the filament surface.
[0013] The term "polymer" includes, but is not limited to, homopolymers, copolymers, such as block, graft, random, and alternating copolymers, terpolymers, and the like, as well as blends and modifications thereof. Furthermore, unless otherwise specifically limited, the term "polymer" is intended to include all possible geometric configurations of the material. These configurations include, but are not limited to, isotactic, syndiotactic, and atactic symmetries. The term "copolymer" refers to a polymer containing two or more different monomer units, thereby including terpolymers, tetrapolymers, and the like.
[0014] The terms "comprises" and "includes" and variations thereof do not have a limiting meaning where these terms appear in the description and claims. Such terms are understood to imply the inclusion of the stated step or element, or group of steps or elements, but not the exclusion of any other step or element, or group of steps or elements. By "consisting of" it is meant to include, but not be limited to, whatever the phrase "consisting of" follows. Thus, the phrase "consisting of" indicates that the recited elements are necessary or required, and that other elements may not be present. By "consisting essentially of" it is meant to include any element recited before the phrase, and is limited to other elements that do not interfere with or contribute to the activity or action specified in this disclosure for the recited element. Thus, the phrase "consisting essentially of" indicates that the recited elements are necessary or required, but that other elements are optional and may or may not be present depending on whether they substantially affect the activity or action of the recited element.
[0015] The words "preferred" and "preferably" refer to embodiments of the present disclosure that may provide certain benefits, under particular circumstances. However, other embodiments may also be preferred, under the same or other circumstances. Furthermore, the recitation of one or more preferred embodiments does not imply that other embodiments are not useful, and is not intended to exclude other embodiments from the scope of the present disclosure.
[0016] In this application, for example, the terms "a," "an," and "the" are not intended to refer only to a singular entity, but include general categories of which specific examples may be used for illustration. The terms "a," "an," and "the" are used synonymously with the term "at least one."
[0017] The phrases "at least one of" and "comprising at least one of" following a list refer to any one of the items in the list, and any combination of two or more items in the list.
[0018] As used herein, the term "or" is generally used in its ordinary sense, including "and / or," unless the content clearly dictates otherwise. The term "and / or" refers to one or all of the listed elements or a combination of any two or more of the listed elements.
[0019] Similarly, all numbers herein are deemed to be modified by the term "about," and preferably by the term "exactly." When used herein in connection with a measured quantity, the term "about" refers to a variation in the measured quantity that can be expected by the skilled artisan making the measurement and exercising a certain level of care, commensurate with the precision of the measurement and the measuring device being used.
[0020] Similarly, herein, the recitations of numerical ranges by endpoints include not only the endpoints but all numbers subsumed within that range (e.g., 1 to 5 includes 1, 1.5, 2, 2.75, 3, 3.80, 4, 5, etc.). As used herein, a number that is "up to" is inclusive of the number (e.g., 50).
[0021] The terms "in the range" or "within a range" (and similar descriptions) include the endpoints of the stated range.
[0022] Throughout this specification, references to "one embodiment," "an embodiment," "particular embodiment," "some embodiments," or the like mean that the particular features, configurations, compositions, or characteristics described in connection with an embodiment are included in at least one embodiment of the invention. Thus, the appearances of such phrases in various places throughout this specification do not necessarily refer to the same embodiment of the invention. Furthermore, the particular features, configurations, compositions, or characteristics may be combined in any suitable manner in one or more embodiments.
[0023] The above summary of the present disclosure is not intended to describe each disclosed embodiment or every implementation of the present disclosure. The following description more particularly illustrates exemplary embodiments. In several places throughout the application, guidance is provided through lists of examples, which examples can be used in various combinations. In each instance, the recited list serves only as a representative group and should not be interpreted as an exclusive list.
[0024] The present disclosure may be more fully understood in connection with the following drawings. [Brief description of the drawings]
[0025] [Figure 1] 1 is a cross-sectional view of a portion of an embodiment of a composite filter media of the present disclosure. [Diagram 2]1 is a cross-sectional view of an embodiment of a composite filter media of the present disclosure. [Diagram 3] 1 is a cross-sectional view of an embodiment of a composite filter media of the present disclosure. [Figure 4] FIG. 1 is a perspective view of one embodiment of a filter element that can be used in an air intake system. [Diagram 5] FIG. 13 is a perspective view of another embodiment of another element comprising a filter media of the present disclosure. [Figure 6] FIG. 13 is a top plan view of another filter element of the present disclosure that can be used in an air intake. [Figure 7] FIG. 7 is a front elevation view of the element of FIG. [Figure 8] FIG. 8 is a right side view of the filter element of FIG. 7. [Figure 9] 1 is a schematic cross-sectional view of a further embodiment of a filter element. [Figure 10] 1 is a schematic cross-sectional view of a further embodiment of a filter element. [Figure 11] 1 is a schematic cross-sectional view of a further embodiment of a filter element. [Figure 12] 1 is a schematic cross-sectional view of a further embodiment of a filter element. [Figure 13] 1 is a schematic cross-sectional view of a further embodiment of a filter element. [Figure 14] FIG. 2 is a perspective view of another embodiment of a filter element. [Figure 15] FIG. 2 is a perspective view of another embodiment of a filter element having an oval configuration. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0026] The present disclosure provides filter media and filter elements, particularly for gas (eg, air) filtration applications.
[0027] In one embodiment, a gas filter media (eg, air filter media) comprising a surface loaded filter layer comprising fine fibers having an average diameter of less than 1 micron, a depth loaded filter layer, and a support layer.
[0028] In use, the layers are constructed and arranged for placement in a gas stream with the surface-loaded filter layer being the most upstream layer, i.e., the layers are positioned relative to one another such that the surface-loaded filter layer (i.e., the fine fiber filter layer) is positioned as the first layer encountered by the gas (e.g., air) stream being filtered (i.e., the fine fiber filter layer is the most upstream layer).
[0029] In certain embodiments, the filter media of the present disclosure are pulse-cleanable. Pulse-cleanability is important for self-cleaning (e.g., via a back pulse of air) and is useful when the filter media is used for very high dust concentrations. Pulse-cleanability can be determined according to the modified ISO 11057 test method described in the Examples section.
[0030] In certain embodiments, the composite filter media includes two or more fine fiber filter layers. In certain embodiments, the composite filter media includes two or more depth load layers (e.g., glass-containing filter layers, meltblown filter layers, or combinations thereof). In certain embodiments, the composite filter media includes two or more support layers. These layers can be arranged in various orders, so long as one of the fine fiber filter layers is the most upstream layer.
[0031] Each filter layer and support layer may be a composite of multiple layers, for example, the deep load layer may be a composite of two or more different layers of meltblown fibers that differ in either composition and / or fiber diameter.
[0032] In certain embodiments, the filter media of the present disclosure have a thickness of at least 10 mils (0.25 mm). In certain embodiments, the filter media of the present disclosure have a thickness of at most 60 mils (1.5 mm), or at most 30 mils (0.76 mm).
[0033] As shown in FIG 1, which illustrates a portion of an exemplary composite filter media 10 of the present disclosure, there are at least two filter layers, i.e., layers that perform filtration: a surface-loaded layer 20, and a depth-loaded filter layer (e.g., a glass-containing filter layer) 22. In one embodiment, as shown in FIG 2, which illustrates an exemplary composite filter media 10 of the present disclosure, there is a surface-loaded layer 20, a depth-loaded filter layer (e.g., a glass-containing filter layer) 22, and a support layer 18 positioned between the depth-loaded layer 22 and the surface-loaded layer 20. In another embodiment, as shown in FIG 3, which illustrates an exemplary composite filter media 10 of the present disclosure, there is a support layer 18, a surface-loaded layer 20, and a depth-loaded filter layer (e.g., a glass-containing filter layer) 22 positioned between the support layer 18 and the surface-loaded layer 20.
[0034] As shown in these exemplary embodiments, surface-loaded filtration layer 20 is positioned upstream of depth-loaded filtration layer 22 relative to the direction of gas flow (e.g., air flow) indicated by the arrows, i.e., surface-loaded filtration layer 20 is the first layer encountered by the gas (e.g., air) flow during use.
[0035] The thickness of each of the filter and support layers may be the same or different and is not limiting. However, it should be noted that the thickness affects the filtration characteristics. The overall thickness of the media is desirably minimized without significantly affecting other media properties such as dust loading capacity, efficiency, and permeability. This, for example, preferably allows for more pleats in the element so that the filter element contains the maximum amount of media without adversely affecting the properties and performance of the filter element (e.g., efficiency, pressure drop, or dust loading capacity).
[0036] Typically, in the filter media of the present disclosure, the filter layer, preferably the filter layer and the support layer, are bonded together with adhesives, binder fibers, thermal bonding, ultrasonic bonding, self-adhesive, or using a combination of such techniques. Preferred methods include the use of adhesives, binder fibers, or combinations thereof. Particularly preferred methods are by the use of adhesives (pressure sensitive adhesives, hot melt adhesives) that are applied in a variety of techniques, including powder coating, spray coating, or the use of preformed adhesive webs. Typically, the adhesive is in a continuous layer, or the adhesive can be patterned, if desired, as long as the filter media does not delaminate during processing or use. Exemplary adhesives include hot melt adhesives, such as polyesters, polyamides, acrylates, or combinations thereof (blends or copolymers).
[0037] If an adhesive is used, the amount of adhesive can be readily determined by one of ordinary skill in the art. The desired level is one that provides a suitable bond between the layers without adversely affecting gas flow through the media. For example, the reduction in Frazier permeability of a composite filter media is the inverse of the sum of the inverses of the permeabilities of each layer (i.e., (1 / A perm +1 / B perm +1 / C perm ) -1 ) is preferably less than 20%, or more preferably less than 10%. This is also applicable to any other lamination method.
[0038] Filter media may be corrugated to increase stiffness and provide better flow channels in the element. Thus, in certain embodiments, the filter media of the present disclosure must possess the characteristics to undergo a typical heat corrugation process without media damage (which often compromises media performance).
[0039] With or without corrugations, the filter media can be folded into multiple folds or pleats and then installed in a filter housing or frame. Pleating of the flat or corrugated sheet can be performed using any number of pleating techniques, including but not limited to rotary pleating, blade pleating, and the like. The corrugated media may have any one of several pleat support mechanisms applied to pleated media described in U.S. Pat. No. 5,306,321. For example, corrugated aluminum separators, hot melt beads, and press fits (often referred to as PLEATLOC pleated media) can be used.
[0040] In certain embodiments, folds are cut into the filter media in a spacer shape, so that even when the media is wet or over-packed, the folds are prevented from joining in an effective manner. These indent the pleat tips perpendicular to the corrugation channel direction on both sides of the media, keeping the pleats separated and providing better flow channels for gas (e.g., air) to flow through the pleat pack in the element. In the case of cone- or cylindrical-type elements, such as those shown in Figures 9-14, the outer indentations can be deeper and wider than the inner indentations to keep the pleats evenly separated.
[0041] For non-corrugated media, other pleat separation methods may be used with any of the media described herein, such as those involving the addition of hot melt adhesive beads between the pleats or the use of comb separators. The pleated material may be formed into a cylinder or "tube" and then bonded together, for example, through the use of an adhesive (such as a urethane-based hot melt adhesive), or ultrasonic welding (i.e., ultrasonic bonding), or the like.
[0042] In certain embodiments, the filter layers, composite filter media (flat or corrugated), and filter elements of the present disclosure are referred to as "high efficiency". In certain embodiments, the high efficiency filter layers of the present disclosure are capable of removing at least 55%, at least 70%, at least 80%, at least 85%, at least 95%, at least 99.5%, at least 99.95%, or at least 99.995% (by number) of 0.4 micron sized DEHS particles at 4 ft / min (2 cm / sec). In certain embodiments, the high efficiency composite filter media (which may or may not be corrugated) and / or filter elements (which are typically corrugated and pleated) of the present disclosure exhibit an efficiency of at least F9 according to EN779:2012. In certain embodiments, the high efficiency filter elements of the present disclosure (which are typically corrugated and pleated) exhibit an efficiency of at least E10, at least E11, or at least E12 according to EN1822:2009.
[0043] In certain embodiments, the filter media exhibits an efficiency of at least 80%, or greater than 80%, according to the DEHS efficiency test for most penetration particle sizes.
[0044] In certain embodiments, the filter layers and / or composite filter media of the present disclosure have good depth loading characteristics.
[0045] In certain embodiments, the depth-loading filter layer has a relatively low toughness. As used herein, toughness is the solid fiber volume divided by the total volume of the filter media in question, and is usually expressed as a percentage, or in other words, as the ratio of fiber volume per unit mass divided by media volume per unit mass. Suitable tests for determining toughness are described, for example, in U.S. Patent Application Publication No. 2014 / 0260137. Typically, the toughness is less than 20 percent (i.e., 0.1 kg / cm) at a pressure of 1.5 pounds per square inch (psi). 2), or in many cases less than 15% robustness is desired.
[0046] In certain embodiments, the filter layers and / or composite filter media of the present disclosure exhibit high strength and flexibility, which may be indicated by a relatively low loss in tensile strength after the layers and / or composite media are folded or corrugated. It is desirable for the filter layers or filter media to lose less than 20% of their tensile strength after folding or corrugating.
[0047] Surface Load Filter Layer A surface-loaded filter layer is a filter layer that traps a significant portion of incident particles at the surface of the layer, as opposed to the volume or thickness of the filter layer (i.e., in the "z" direction). That is, a surface-loaded filter layer can stop incident particles from passing through the surface-loaded filter layer, while also achieving a significant surface load due to the trapped particles.
[0048] The surface-loaded filter layer of the filter media of the present disclosure comprises fine fibers having an average fiber diameter of less than 1 micron (i.e., 1000 nanometers), or at most 0.5 microns, or at most 0.3 microns. This includes nanofibers and microfibers. Nanofibers are fibers having a diameter of less than 200 nanometers or 0.2 microns. Microfibers are fibers having a diameter of more than 0.2 microns and not more than 10 microns. In certain embodiments, the fine fibers have an average diameter of at least 0.01 microns, or at least 0.05 microns, or at least 0.1 microns.
[0049] In certain embodiments, the surface loaded filter layer has a surface area of 1 gram per square meter (g / m 2 or gsm). In certain embodiments, the surface load filter layer has a basis weight of at least 0.0001 g / m 2 The basis weight is
[0050] In certain embodiments, the surface loaded filter layer has a LEFS filtration efficiency of at least 30%, at least 40%, at least 50%, at least 60%, at least 70%, or at least 80%. In certain embodiments, the fine fiber filter layer has a LEFS filtration efficiency of at most 99%, at most 98%, at most 97%, at most 96%, at most 95%, at most 94%, at most 93%, at most 92%, at most 91%, or at most 90%.
[0051] Examples of fine fibers are disclosed in US Pat. No. 8,118,901.
[0052] The surface-loaded filter layers of the present disclosure may include a random distribution of fine fibers that may be bonded to form an interlocking net. Filtration performance is achieved in large part as a result of the shielding of the fine fibers against particulate passage. The structural properties of stiffness, strength, and pleatability are typically provided by a support layer (e.g., a support layer to which the fine fibers are adhered) contained within the filter media.
[0053] In certain embodiments, the surface-loaded filter layer may include an interlocking network of fine fibers. Such a network typically includes fine fibers in the form of microfibers or nanofibers, with relatively small spaces between the fibers. Such spaces typically range from 0.01 microns to 25 microns, or often 0.1 microns to 10 microns, between the fibers.
[0054] In certain embodiments, the fine fibers add less than 1 micron thickness to the overall filter media. In service, the filter is capable of stopping incident particles from passing through the surface-loaded filter layer while achieving significant surface loading with trapped particles. Particles, including dust or other incident particles, rapidly form a dust cake on the fine fiber surface while maintaining high initial and overall efficiency of particle removal. Even with relatively fine contaminants having particle sizes between 0.01 micron and 1 micron, filter media containing fine fibers have extremely high dust carrying capacity.
[0055] Suitable polymeric materials useful for making fine fibers have substantially improved resistance to the undesirable effects of heat, humidity, high flow rates, back pulse cleaning, operational abrasion, submicron particles, filter cleaning during use, and other demanding conditions.
[0056] Examples of polymeric materials that are microfibers and their composition are disclosed in U.S. Patent No. 8,118,901. Such polymeric materials include both addition and condensation polymeric materials, such as polyolefins, polyacetals, polyamides, polyesters, cellulose ethers and esters, polyalkylene sulfides, polyarylene oxides, polysulfones, modified polysulfone polymers, and mixtures thereof. Preferred materials within these general categories include polyethylene, polypropylene, poly(vinyl chloride), polymethyl methacrylate (and other acrylics), polystyrene, and copolymers thereof (including ABA type block copolymers), poly(vinylidene fluoride), poly(vinylidene chloride), polyvinyl alcohol, in crosslinked and uncrosslinked forms, with various degrees of hydrolysis (87% to 99.5%). Preferred addition polymers tend to be glassy (Tg above room temperature). This is the case for polyvinyl chloride and polymethyl methacrylate, polystyrene polymer compositions or alloys thereof, or for polyvinylidene fluoride and polyvinyl alcohol materials.
[0057] One class of polyamide condensation polymers is nylon materials. The term "nylon" is a generic name for all long-chain synthetic polyamides. Typically, nylon nomenclature includes a sequence of numbers, such as in nylon-6,6, indicating that the starting materials are C6 diamines and C6 diacids (the first number indicates the C6 diamine and the second number indicates the C6 dicarboxylic acid compound). Another nylon can be made by polycondensation of ε-caprolactam in the presence of small amounts of water. This reaction forms nylon-6 (made from a cyclic lactam also known as ε(episilon)-aminocaproic acid), a linear polyamide. Additionally, nylon copolymers are also envisioned.
[0058] Copolymers can be made by combining various diamine compounds, various diacid compounds, and various cyclic lactam structures in a reaction mixture, then forming nylon with the monomeric materials randomly positioned in the polyamide structure. For example, nylon 6,6-6,10 material is made by combining hexamethylene diamine and the C6 and C7 diacids. 10 Nylon 6-6,6-6,10 is a nylon made from a blend of ε-aminocaproic acid, hexamethylenediamine, and C6 and C 10 It is a nylon made by copolymerization of a blend of diacid materials.
[0059] Block copolymers are also useful in making fine fibers. With such copolymers, the choice of solvent swelling agent is important. The solvent selected is such that both blocks are soluble in the solvent. An example is ABA (styrene-EP-styrene) or AB (styrene-EP) polymers in methylene chloride solvent. If one component is not soluble in the solvent, it forms a gel. Examples of such block copolymers are KRATON copolymers of styrene-b-butadiene and styrene-b-hydrogenated butadiene (ethylene propylene), PEBAX copolymers of e-caprolactam-b-ethylene oxide, SYMPATEX polyester-b-ethylene oxide, and polyurethanes of ethylene oxide and isocyanates.
[0060] Addition polymers such as polyvinylidene fluoride, syndiotactic polystyrene, copolymers of vinylidene fluoride and hexafluoropropylene, polyvinyl alcohol, polyvinyl acetate, amorphous addition polymers such as poly(acrylonitrile) and its copolymers with acrylic acid and methacrylate, polystyrene, poly(vinyl chloride) and its various copolymers, poly(methyl methacrylate) and its various copolymers can be solution spun relatively easily because they are soluble at low pressures and temperatures. However, highly crystalline polymers such as polyethylene and polypropylene require high temperature, high pressure solvents if they are to be solution spun. Therefore, solution spinning of polyethylene and polypropylene is extremely difficult. Electrostatic solution spinning is one method of making fine fibers.
[0061] In certain embodiments, the microfibers comprise a single polymeric material. In certain embodiments, the microfibers comprise a polymeric mixture comprising a first polymer conditioned or processed at high temperature and a second, different polymer (different polymer type, molecular weight or physical properties). The polymeric mixture can be reacted or formed into a single chemical species or physically combined into a blended composition by an annealing process. Annealing results in physical changes such as crystallization, stress relaxation or orientation. In certain embodiments, the polymeric materials are chemically reacted into a single polymeric species such that differential scanning calorimetry analysis reveals a single polymeric material. Compatible mixtures of similar polymers, such as blends of similar nylons, similar polyvinyl chloride polymers, polyvinylidene chloride polymers, are useful in surface-loaded filter layer fibers.
[0062] In certain embodiments, the microfibers comprise nylon, polyvinylidene fluoride, polyurethane, or combinations thereof (eg, blends or copolymers).
[0063] Additive materials may also be used to form surface coatings on the microfibers that provide oleophobic, hydrophobic, or other related improved stability when exposed to high temperatures, high humidity, and difficult operating conditions. Such microfibers may have a smooth surface that includes a separate layer of additive material, or an outer coating of additive material partially solubilized or alloyed in the polymer surface, or both.
[0064] Additives include fluorosurfactants, nonionic surfactants, low molecular weight resins, such as tertiary butyl phenol resins with molecular weights less than about 3000. This resin is characterized by oligomeric junctions between phenol nuclei in the absence of methylene bridging groups. The positions of the hydroxyl and tertiary butyl groups can be randomly positioned around the ring. The junctions between phenol nuclei always occur next to the hydroxyl groups and do not occur randomly. Similarly, the polymeric material can be combined with alcohol-soluble nonlinear polymeric resins formed from bisphenol A. Such materials are similar to the tertiary butyl phenol resins described above in that they are formed using oligomeric junctions that directly connect aromatic rings to aromatic rings without bridging groups such as alkylene or methylene groups.
[0065] In certain embodiments, the polymer and optional additives are selected to provide temperature resistance, moisture resistance, and solvent resistance. In certain embodiments, the polymer material and optional additives are selected to survive various operating temperatures, i.e., 140°F, 160°F, 270°F, 300°F, for 1-3 hours, depending on the end use, while retaining 30%, 50%, 80%, or 90% of the filter efficiency or the effective fine fibers in the filter layer, without damage. Survival at these temperatures is important at low humidity, high humidity, and in water-saturated gas (e.g., air).
[0066] In certain embodiments, the polymer and optional additives are selected to provide adhesion of the material to the remainder of the media structure such that the composite media can be processed into filter structures, tubular materials, and other structures, including pleats, without significant delamination.
[0067] The fine fiber filter layer may comprise a bi- or multi-layer structure, where the filter contains one or more surface-loaded filter layers combined or separated by one or more synthetic, cellulosic, or blended webs. Another preferred motif is a structure that includes fine fibers in a matrix or blend of other fibers.
[0068] For pulse cleaning applications, a very thin layer of fine fibers can help minimize pressure loss and provide an outer surface for particle capture and release. A thin layer of fibers less than 1 micron in diameter, or less than 0.5 microns in diameter, is preferred for self-cleaning applications. Good adhesion between the fine fibers and adjacent layers (e.g., deep-loading layers) is important. Self-cleaning the surface by repeatedly back-pulsing restores the filter media. When large forces are applied to the surface, fine fibers with poor adhesion to the substrate can peel off during back-pulsing from the interior of the filter through the substrate to the surface-loading filter layer.
[0069] deep load layer A deep-loaded layer is a filter layer that traps particles throughout the volume of the layer, so that debris is trapped throughout the thickness of the filter layer (i.e., in the "z" direction) as opposed to on the surface of a surface-loaded filter layer.
[0070] Deep load layers are often characterized in terms of their porosity, density, and solids percentage. For example, 5% rigid media means that about 5% of the total volume contains solids (e.g., fibrous materials), with the remainder being void space filled with air or other fluids.
[0071] In certain embodiments, the depth load filter layer has a relatively low toughness. Typically, the depth load filter layer has a toughness of 1.5 psi (i.e., 0.1 kg / cm 2 In certain embodiments, the depth load filter layer of the present disclosure has a robustness of less than 20 percent (%), and often less than 15%, at a pressure of 1.5 psi (i.e., 0.1 kg / cm). 2 ) has a toughness of at least 5 percent at a pressure of
[0072] In certain embodiments, the depth load filter layer has a resistance to moisture of at least 8 liters per square meter per second (l / m) when rated separately from the remainder of the structure. 2 / sec), at least 20 l / m 2 / sec, at least 40 l / m 2 / sec, at least 80 l / m 2 / sec, at least 100 l / m 2 / sec, or at least 200 l / m 2 / sec Frazier permeability (pressure difference set at 0.5 inches of water). In certain embodiments, the depth load filter layer, when rated separately from the rest of the structure, has a maximum permeability of 1000 l / m 2 -sec, up to 800 l / m 2 -sec, up to 600 l / m 2 -sec, up to 400 l / m 2 -sec, or up to 200 l / m 2 / sec Frazier permeability (pressure difference set at 0.5 inches of water).
[0073] Another commonly used depth-loading filter layer characteristic is fiber diameter. Generally, the smaller the fiber diameter for a given firmness percentage, the more efficient the filter media will be in its ability to capture smaller particles. Given the fact that smaller fibers take up less volume than larger fibers, smaller fibers can be packed in greater numbers without increasing the overall firmness percentage.
[0074] Because the depth-loading filter layer captures particles substantially throughout the entire volume or depth, such filter layers can be loaded with higher weights and volumes of particles over the life of the filter media compared to surface-loading filter layers. However, depth-loading filter layers tend to be less efficient than surface-loading filter layers. To facilitate such high loading capacity, low-rigidity depth-loading filter layers are often selected for use. This can result in a large average pore size, which may allow some particles to pass through the filter more easily. Adding a graded density system and / or a surface-loading filter layer can provide improved efficiency characteristics.
[0075] In certain embodiments, the depth loading layer of the filter media of the present disclosure is a high efficiency filter layer. In certain embodiments, the high efficiency filter layer exhibits a filtration efficiency of at least 55%, or at least 70% for 0.4 micron size DEHS (Di-Ethyl-Hexyl-Sebacate) particles at 4 ft / min (2 cm / sec). Preferably, the filtration efficiency is at least 80%, at least 85%, at least 95%, at least 99.5%, at least 99.95%, or at least 99.995% for most penetrating particle size (MPPS) particles at 4 ft / min (2 cm / sec).
[0076] In certain embodiments, the deep loading layer exhibits a filtration efficiency of up to 99%, up to 99.5%, up to 99.97%, or up to 99.997% with 0.4 micron sized DEHS (di-ethyl-hexyl-sebacate) particles at 4 ft / min (2 cm / sec).
[0077] In certain embodiments, the depth loading filter layer of the present disclosure has a terminal pressure drop of at least 1 gram per square meter (g / m) at 2 inches of water column rise to an initial value (i.e., 500 Pa). 2 or gsm), at least 2g / m 2 , at least 3 g / m2 , at least 4 g / m 2 , at least 5 g / m 2 , at least 6 g / m 2 , at least 7 g / m 2 , at least 8 g / m 2 , at least 9 g / m 2 , or at least 10 g / m 2 This represents the salt loading capacity of the depth loaded filter layer at a maximum of 10 g / m2 at a pressure increase of 500 Pascals relative to the initial value. Typically, the higher the salt loading capacity, the better, as this is an indication of the life of the product. In certain embodiments, the depth loaded filter layer has a salt loading capacity of up to 10 g / m2 at a pressure increase of 500 Pascals relative to the initial value. 2 represents the salt loading capacity of
[0078] In certain embodiments, the deep load layer is at least 0.005 inches (125 microns) thick, and often at least 0.01 inches (250 microns) thick. In certain embodiments, the deep load layer is at most 0.02 inches (500 microns) thick.
[0079] In certain embodiments, the depth load filter layer has a thickness of at least 10 g / m 2 , at least 20 g / m 2 , at least 30 g / m 2 , at least 40 g / m 2 , or at least 50 g / m 2 In certain embodiments, the depth load filter layer has a basis weight of up to 150 g / m 2 , up to 140 g / m 2 , up to 130 g / m 2 , up to 120 g / m 2 , up to 110 g / m 2 , up to 100 g / m 2 The basis weight is
[0080] In a particular embodiment, the deep loading layer has a water resistance of at least 0.5 g / ft2 at 2 inches water rise and 10 ft / min (5.8 cm / sec) with 0.3 micron NaCl particles. 2 (5.4g / m 2) dust loading capacity. In a particular embodiment, the deep loading layer is capable of withstanding up to 5 g / ft 2 of 0.3 micron NaCl particles at 2 inches of water rise and 10 ft / min (5.8 cm / sec). 2 (53.8g / m 2 ) represents the dust load capacity.
[0081] In certain embodiments, the depth load layer comprises a glass-containing filter layer, a meltblown filter layer, or a combination thereof.
[0082] In certain embodiments, the depth load layer comprises a glass-containing filter layer. In certain embodiments of glass-containing filter layers, such layers comprise glass fibers having an average diameter of at most 2 microns, at most 1 micron, or at most 0.5 microns. In certain embodiments, the glass fibers have an average diameter of at least 0.01 microns, at least 0.05, at least 0.1 microns, at least 0.2 microns, at least 0.3 microns, or at least 0.4 microns.
[0083] The glass-containing filter layer may also contain fibers other than glass-containing fibers. For example, it may contain multicomponent fibers, typically bicomponent fibers, that function as binder fibers. A preferred example is a bicomponent binder fiber that is a core-sheath fiber, with a low melting point polyester sheath and a higher melting point polyester core. Bicomponent fibers typically have a fiber diameter of at least 10 microns.
[0084] The glass-containing filter layer may also include polyester fibers different from the multicomponent fibers. A preferred glass-containing filter layer of the present disclosure includes only glass fibers and bicomponent binder fibers. In a particular embodiment, the polyester fibers different from the multicomponent binder fibers have an average diameter of 10 microns to 14 microns.
[0085] The fibers of the glass-containing filter layer can be made by a variety of processes, hi certain embodiments, the glass-containing filter layer is produced using a wet process.
[0086] The binder fibers in the glass-containing filter layer are used to avoid the use of binder resins, although such resins may be added to further improve its strength. Examples of suitable binder resins include solvent-based or water-based latex resins, water-based styrene acrylics, solvent-based phenolic resins, and solvent-based non-phenolic resins, such as those available under the trademark HYCAR26138 from Lubrizol of Cleveland, OH. Typically, when used, binder resins may be present in the glass-containing filter layer in an amount of up to 10% by weight, up to 5% by weight, or up to 1% by weight based on the total weight of the glass-containing filter layer. Preferably, no binder resin is used in the glass-containing filter layer (or in any of the layers of the filter media).
[0087] Examples of suitable glass-containing filter layers include those described in U.S. Pat. Nos. 7,309,372, 7,314,497, 7,985,344, 8,057,567, and 8,268,033, as well as U.S. Patent Application Publication Nos. 2006 / 0242933 and 2008 / 0245037.
[0088] In certain embodiments, the depth load layer comprises a meltblown filter layer. Typically, meltblown lamination is a nonwoven web forming process in which molten polymer resin is extruded and pulled with a heated, high velocity gas (e.g., air) to form fine filaments. The filaments are cooled and collected as a web onto a moving screen. This process is similar to the spun-bond process, but meltblown fibers are typically much finer.
[0089] Typically, the meltblown fibers have an average diameter of 20 microns or less. In certain embodiments, the meltblown filter layer comprises meltblown fibers having an average diameter of at most 10 microns, at most 5 microns, at most 4 microns, or at most 3 microns. In certain embodiments, the meltblown filter layer comprises meltblown fibers having an average diameter of at least 0.5 microns, at least 1 micron, at least 1.5 microns, or at least 2 microns. In certain embodiments, the meltblown fibers have an average diameter of 2 to 3 microns.
[0090] In certain embodiments, scaffold fibers as described in WO2013 / 025445 can be included in the meltblown filter layer as needed to enhance performance.However, media with high compressibility have little or no scaffold fibers as described in WO2013 / 025445 used in the meltblown filter layer.Scaffold fibers provide support for media fibers, adding improved handling, greater tensile strength, and resulting in lower compressibility for the media.
[0091] In certain embodiments, the meltblown filter layer comprises a continuously tapered structure of larger fibers and a more open structure on a first major surface, and a smaller fiber and a less open structure on a second major surface. In certain embodiments of this structure, the second major surface of the meltblown filter layer is adjacent to the support layer, and the first major surface is positioned as the most upstream surface (i.e., the first layer encountered by the gas (e.g., air) flow during use).
[0092] In certain embodiments, the meltblown filter layer comprises a composite of multiple layers of meltblown fibers with larger fibers and a more open structure on a first major surface of the meltblown composite and smaller fibers and a less open structure on a second major surface of the meltblown composite. In certain embodiments of this structure, the second major surface of the meltblown filter layer is adjacent to the support layer and the first major surface is positioned adjacent to the surface-loaded filter layer.
[0093] In certain embodiments, meltblown fibers can be prepared from a variety of polymers suitable for meltblown lamination. Examples include polyolefins (particularly polypropylene), ethylene-chloro-trifluoroethylene, other hydrophobic polymers, or non-hydrophobic polymers with hydrophobic coatings or additives (e.g., polybutylene terephthalate, polystyrene, polylactic acid, polycarbonate, nylon, polyphenylene sulfide), or combinations thereof (e.g., blends or copolymers). Preferred polymers are polyolefins, such as polypropylene, polyethylene, and polybutylene.
[0094] In certain embodiments, the meltblown filter layer comprises fibers made of polypropylene, polybutylene terephthalate, or combinations thereof. Particularly preferred meltblown fibers are made of polypropylene to enhance the watertight characteristics of the preferred filter media of the present disclosure.
[0095] In certain embodiments, the meltblown filter layer is hydrophobic. By this, it is meant that the layer exhibits a contact angle with water of greater than 90 degrees. The material, the fibrous material, may be hydrophobic (e.g., polyolefin), or may contain a hydrophobic additive, or may be coated with a hydrophobic material. Similarly, in certain embodiments, the glass-containing filter layer is coated with a hydrophobic coating to enhance the watertight characteristics. Alternatively, the deep-load filter layer may be treated with a plasma treatment technique.
[0096] Suitable hydrophobic materials have little or no affinity for water or repel water completely, thereby preventing or limiting the passage of water through the filter media. Typically, hydrophobic materials, when tested, exhibit a contact angle with water of greater than 90 degrees. Examples of hydrophobic materials include fluorochemicals, particularly the fluoropolymers described in U.S. Pat. No. 6,196,708.
[0097] Examples of useful fluoropolymers include those having fluoroalkyl or, preferably, perfluoroalkyl moieties. These fluoropolymers include, for example, fluoroalkyl esters, fluoroalkyl ethers, fluoroalkyl amides, and fluoroalkyl urethanes. Often, the fluoroalkyl and / or perfluoroalkyl moieties extend from the backbone of the polymer.
[0098] Fluoropolymers can include various monomer units. Exemplary monomer units include, for example, fluoroalkyl acrylates, fluoroalkyl methacrylates, fluoroalkyl aryl urethanes, fluoroalkyl aryl urethanes, fluoroalkyl maleates, fluoroalkyl urethane acrylates, fluoroalkyl amides, fluoroalkyl sulfonamide acrylates, and the like. Fluoropolymers can optionally have additional non-fluorine-based monomer units, including unsaturated hydrocarbons (e.g., olefins), acrylates, and methacrylates, and the like. Additional examples of suitable fluoropolymers are provided in U.S. Pat. No. 3,341,497.
[0099] Commercially available fluoropolymers include those available under the trade designation OLEOPHOBOL CPX from Huntsman (Charlotte, NC), as well as 3M Protective Material PM-490 (a non-ionic fluorochemical resin), 3M Protective Material PM-3633 (a fluoropolymer emulsion), 3M L-21484 (a fluorinated amino salt derivative that can be diluted in water or polar organic solvents), all of which are available from 3M Co. (St. Paul, MN).
[0100] Other exemplary commercially available fluoropolymers are provided in aqueous emulsions. The fluoropolymers can be extracted from the aqueous emulsions by removal of the water carrier. The fluoropolymers can then be solvated in organic solvents. To facilitate solvation of the fluoropolymers, a compound such as acetone can be optionally added to the aqueous emulsion to break the emulsion. In addition, the fluoropolymer particles can be optionally ground after removal of the water to make solvation easier and faster.
[0101] Methods for coating such materials are recognized and known to those skilled in the art. Typical coating weights are at least 0.5% by weight, and often no more than 3% by weight.
[0102] support layer The filter media of the present disclosure includes a support layer. The support layer can be any of a variety of porous materials, including fibrous materials, metal mesh, and the like. Typically, the fibrous material used for the support layer is made of natural and / or synthetic fibers. It can be woven or nonwoven. It can be spunbond, wetlaid, and the like.
[0103] In certain embodiments, the support layer comprises fibers having an average diameter of at least 5 microns, or at least 10 microns, hi certain embodiments, the support layer may comprise fibers having an average diameter of up to 250 microns.
[0104] In certain embodiments, the support layer has a modulus of at least 50 grams per square meter (g / m 2 or gsm), or at least 100 gsm. In certain embodiments, the support layer has a basis weight of at most 260 grams per square meter (g / m 2 or gsm), up to 200 g / m 2 , or up to 150 g / m 2 The basis weight is
[0105] In certain embodiments, the support layer is at least 0.005 inches (125 microns) thick, and often at least 0.01 inches (250 microns) thick. In certain embodiments, the support layer is at most 0.03 inches (750 microns) thick.
[0106] In certain embodiments, the support layer has a flow rate of at least 10 cubic feet per minute (ft 3 ) at 125 Pa when rated separately from the remainder of the structure. 3 / min) (80.2 l / m at 200 Pa 2 / sec. In certain embodiments, when rated separately from the rest of the structure, it has a maximum permeability of 1000 cubic feet per minute (ft 3 ) at 125 Pa. 3 / min) (8020 l / m at 200 Pa 2 / s) transparency.
[0107] In certain embodiments, the support layer has a Gurley stiffness of at least 1000 grams, often at least 5000 grams. In certain embodiments, the support layer may have a Gurley stiffness of up to 10,000 grams. Methods for measuring Gurley stiffness are described in TAPPI No. T543.
[0108] Examples of suitable materials for the support layer (i.e., substrate) include spunbond, wet-laid, carded, or meltblown nonwovens. Suitable fibers can be cellulosic, glass, metal, or synthetic polymer fibers or combinations. The fibers can be in the form of woven or nonwoven fabrics. Plastic or metal screen-like materials, both extruded and perforated, are other examples of filter substrates. Examples of synthetic nonwoven fabrics include polyester nonwoven fabrics, nylon nonwoven fabrics, polyolefin (e.g., polypropylene) nonwoven fabrics, polycarbonate nonwoven fabrics, or blended or multicomponent nonwoven fabrics thereof. Sheet-like substrates (e.g., cellulosic, synthetic, and / or glass or combination webs) are typical examples of filter substrates. Other preferred examples of suitable substrates include spunbond polyester or bicomponent polyester fibers (as described herein for glass-containing filter layers) or polypropylene / polyethylene terephthalate, or polyethylene / polyethylene terephthalate bicomponent fibers.
[0109] In certain embodiments, the support layer comprises wet-laid fibers, hi certain embodiments, the support layer comprises wet-laid cellulosic fibers, polyester fibers, or a combination thereof.
[0110] In certain embodiments, the support layer is hydrophobic. The fibrous material may be hydrophobic (e.g., polyolefin), may contain hydrophobic additives, may be coated with hydrophobic materials, such as those described herein for hydrophobic coatings of glass-containing filter layers, or may be treated with plasma treatment techniques. Alternatively, in the case of wet processing, the hydrophobic resin may be applied during the wet process.
[0111] Optional scrim layer In certain embodiments, a scrim layer may be used to increase the stiffness of the filter media of the present disclosure. Typically, the scrim layer is disposed between the surface-loaded filter layer and the depth-loaded filter layer. Materials useful for the scrim layer typically have high permeability (or "perm") (e.g., 1600 l / m2 / s) and are thin (e.g., less than 0.005 inches) so that they have a minimal effect on planar sheet or filter element performance. Examples of such scrim materials include those available under the trademarks FINON C303NW and FINON C3019 NW from Midwest Filtration of Cincinatti, Ohio. Others are described, for example, in U.S. Patent Application Publication No. 2009 / 0120868.
[0112] Filter Elements and Applications The filter media of the present disclosure can then be manufactured into filter elements (i.e., filtration elements), including, for example, flat panel filters, cartridge filters, or other filtering components (e.g., cylindrical or conical). Examples of such filter elements are described in U.S. Patent Application Publication No. 2014 / 0260142, as well as U.S. Patent Nos. 6,746,517, 6,673,136, 6,800,117, 6,875,256, 6,716,274, and 7,316,723.
[0113] The filter media may be corrugated. Exemplary corrugations are 0.020 to 0.035 inches (0.5 mm to 0.9 mm) deep. The corrugated filter media may typically be pleated to form a pleat pack, which may then be placed into a housing and sealed, as known in the art.
[0114] The filter elements of the present disclosure may be used in industrial filtration, such as in dust collectors, and in commercial and residential HVAC systems.
[0115] 4-14 show various embodiments of the filter element of the present disclosure that can be used in a gas turbine intake system or an industrial air washer.
[0116] In FIG. 4, a pleated panel element 200 is shown in a perspective view. The panel element 200 includes a media pack 202 of pleated media 204. The pleated media 204 may include a filter media as described herein. In the illustrated embodiment, the media pack 202 is held within a frame 206, the illustrated example being a rectangular frame 206. The frame 206 typically includes a gasket (not shown) to allow the element 200 to be sealed against a tube sheet in an air intake system. In FIG. 4, the upstream side of the pleated media 204 with the surface-loaded filter layer is shown at 205, on the same side as the drawn-in gas (e.g., air) indicated by arrow 207. Cleaned gas (e.g., air) emerges from the media 204 from the downstream side of the media, indicated by arrow 208.
[0117] 5 shows a perspective view of a pocket filter element 210. The pocket element 210 includes a layer of filter media 212, which may include a filter media of the present disclosure. In the illustrated embodiment, the pocket element 210 includes a plurality of panel pairs 213, 214, each panel pair 213, 214 forming a V-shaped configuration. The filter media 212 is secured to a frame 216. The frame 216 typically supports a gasket to allow the pocket element 210 to be sealed against a tubesheet. In such an arrangement, the media 212 has an upstream meltblown side 217 that is inside the V and a downstream side 218 that is outside the V.
[0118] 6-8 show diagrams of a mini-pleat or multi-V shaped element 220. The element 220 includes a frame 222 that holds a filter media pack 224 (FIG. 8). The media pack 224 includes a plurality of mini-pleats. The mini-pleats are arranged in panels 226, and the element 220 includes a plurality of mini-pleat panel pairs 227, 228 (FIG. 6) of the media of the present invention, each forming a V-like shape. In FIG. 6, the panel pairs 227, 228 are shown in hidden lines because the top portion of the frame 222 obscures the panel pairs 227, 228. The frame 222 defines a plurality of dirty gas (e.g., air) inlets 229 (FIG. 7) that lead to the interior of each V of each pleated panel pair 227, 228. Each pleated panel pair 227, 228 includes an upstream side 230 that is inside the V and a downstream side 231 that is outside the V.
[0119] Figures 9-14 show various embodiments of tubular, pleated filter elements. Figure 9 shows a cylindrical pleated element 240 having a media pack 242 that may include a filter media of the present disclosure having an upstream side 244 and a downstream side 246. The downstream side 246 is within the interior volume of the element 240.
[0120] FIG. 10 shows two of the cylindrical elements 240 axially aligned so as to be side-by-side end-to-end.
[0121] 11, cylindrical element 240 is axially aligned with partial conical element 250. Partial conical element 250 is a tubular element having a media pack 252 that may include a filter media of the present disclosure. The element has an upstream side 254 and a downstream side 256. Conical element 250 has a first end 258 having a diameter that matches the diameter of cylindrical element 240. Conical element 250 includes a second end 260 having a diameter larger than the diameter of first end 258, thus forming a partial conical shape.
[0122] 12 shows two axially arranged and end-to-end engaged partially conical elements 270, 280. Each of the elements 270 includes a media pack 272, 282 forming a tube that may contain the filter media of the present disclosure. The media packs 272, 282 each have an upstream side 274, 284 and a downstream side 276, 286.
[0123] 13 shows a single conical element 270. The element 270 may be used alone in an intake system for a gas turbine without being installed in an element pair as shown in FIGS.
[0124] 14 is another embodiment of a filter element 290 having a media pack 292 that may include the filter media of the present disclosure. The media pack 292 is pleated and forms a tubular shape. In this embodiment, the tubular shape is an ellipse, and in one exemplary embodiment, the ratio of the minor axis to the major axis of the ellipse is about 0.7 to 0.9. The media 292 includes an upstream side 294 and a downstream side 296.
[0125] 15 is another embodiment of a filter element in the form of an oval structure that may include the filter media of the present disclosure. The filter element includes a filter media 310 having an end cap 320 located at each of a first end 312 and a second end 314 of the filter media 310. The end cap 320 at the first end 312 of the filter media 310 may have an opening that allows access to the interior volume of the filter cartridge. The opposite end cap 320 of the filter media 310 may be closed such that the end cap 320 prevents access to the interior volume of the filter cartridge and such that gas (e.g., air) that enters the interior volume of the filter cartridge through the end cap 320 at the first end 312 of the filter media 310 must exit through the filter media in the filter element.
[0126] 15, in one or more alternative embodiments, both end caps 320 may be open to allow access to the interior volume of the filter element. In one or more embodiments, gaskets 322 may be provided on the end caps 320 to seal the filter cartridge over openings in, for example, a tube sheet, venturi, or other structure through which gas is delivered into the interior volume of the filter element. A tube axis 311 extends through the tubular filter cartridge between the first end 312 and the second end 314. The filter media 310 in the filter cartridges described herein define an exterior surface 316 and an interior surface 318 positioned about the tube axis 311. The interior surface 318 faces toward the interior volume of the filter cartridge 310, and the exterior surface 316 faces away from the interior volume.
[0127] In the filter element of FIG. 15 , end cap 320 may include an alignment feature in the form of, for example, an optional tab 324 within which notch 326 is located. Notch 326 may be sized to receive upper and lower members 352 and 354 of a yoke 350 onto which a filter cartridge may be installed in a filter system. Each of notches 326 may, in one or more embodiments, be described as having an opening facing the interior volume of the filter cartridge, with notch 326 extending toward an interior periphery 328 of end cap 320. While in the illustrated embodiment, each notch 326 is formed with a single tab 324, in one or more alternative embodiments, notch 326 may be formed between two members that protrude from the interior periphery 328 of end cap 320, where the two members forming notch 326 are not the same structural member. The use of two tabs 324 in combination with a yoke 350 having two members 352 and 354 can be beneficial to prevent, or at least limit, rotation of a filter cartridge about its tube axis 311 when installed in the yoke 350 in a filter system. Such filter elements are described in further detail in U.S. Patent Application Publication No. 2014 / 0260142.
[0128] It should be understood that each of the filter elements characterized above and shown in FIGS. 4-15 may be flat media or corrugated media and / or may be operatively installed in an intake system or other ventilation system for a gas turbine.
[0129] In operation, the gas (e.g., air) to be filtered is directed upstream, through a surface-loaded fine fiber filter layer, and then through a downstream filter media in each filter element, typically mounted on a tubesheet. The filter media removes at least a portion of the particulate matter from the gas (e.g., air) stream. After passing through the downstream media, the filtered gas (e.g., air) is then directed to a gas turbine.
[0130] Exemplary embodiments Embodiment 1 is a gas filter media including a surface loaded filter layer including fine fibers having an average diameter of less than 1 micron, a depth loaded filter layer, and a support layer, the layers constructed and arranged for placement in a gas stream with the surface loaded filter layer being the most upstream layer.
[0131] Embodiment 2 is the filter media of embodiment 1 that is capable of being pulse washed.
[0132] Embodiment 3 is the filter media of embodiment 1 or 2, wherein the depth-loading filter layer is positioned between the surface-loading layer and the support layer.
[0133] Embodiment 4 is the filter media of any one of embodiments 1-3, wherein the fine fibers have an average diameter of at most 0.5 microns.
[0134] Embodiment 5 is the filter media of embodiment 4, wherein the fine fibers have an average diameter of at most 0.3 microns.
[0135] Embodiment 6 is the filter media of any one of embodiments 1-5, wherein the fine fibers have an average diameter of at least 0.01 microns.
[0136] Embodiment 7 is the filter media of embodiment 6, wherein the fine fibers have an average diameter of at least 0.1 microns.
[0137] Example 8 is the filter media of any one of Examples 1-7, wherein the fine fibers comprise nylon, polyvinylidene fluoride, polyurethane, or a combination thereof.
[0138] Embodiment 9 is the filter media of any one of embodiments 1-8, wherein the surface loaded filter layer has a LEFS filtration efficiency of at least 30%.
[0139] Embodiment 10 is the filter media of embodiment 9, wherein the surface loaded filter layer has a LEFS filtration efficiency of at least 70%.
[0140] Embodiment 11 is the filter media of embodiment 10, wherein the surface loaded filter layer has a LEFS filtration efficiency of at least 80%.
[0141] Embodiment 12 is the filter media of any one of embodiments 1-11, wherein the surface-loaded filter layer has a LEFS filtration efficiency of up to 99%.
[0142] Embodiment 13 is the filter media of embodiment 12, wherein the surface loaded filter layer has a LEFS filtration efficiency of up to 95%.
[0143] Embodiment 14 is the filter media of embodiment 13, wherein the surface loaded filter layer has a LEFS filtration efficiency of up to 90%.
[0144] Embodiment 15 is the filter media of any one of embodiments 1-14, wherein the depth load filter layer comprises a high efficiency glass-containing filter layer, a high efficiency meltblown filter layer, or a combination thereof.
[0145] Example 16 is the filter media of Example 15, wherein the depth-loading filter layer comprises a high-efficiency glass-containing filter layer comprising glass fibers and multicomponent binder fibers.
[0146] Embodiment 17 is the filter media of embodiment 16, wherein the high efficiency glass-containing layer comprises up to 10 wt. % of a binder resin, based on the total weight of the glass-containing layer.
[0147] Example 18 is the filter media of Example 16 or 17, wherein the multicomponent binder fibers of the high efficiency glass-containing filter layer comprise bicomponent fibers having a low melting point polyester sheath and a higher melting point polyester core.
[0148] Example 19 is the filter media of any one of Examples 16-18, wherein the high efficiency glass-containing filter layer further comprises polyester fibers different from the multicomponent binder fibers.
[0149] Embodiment 20 is the filter media of embodiment 19, wherein the polyester fibers distinct from the multicomponent binder fibers have an average diameter between 10 microns and 14 microns.
[0150] Embodiment 21 is the filter media of any one of embodiments 16-20, wherein the high efficiency glass-containing filter layer comprises glass fibers having an average diameter of 0.4 microns to 0.5 microns.
[0151] Embodiment 22 is the filter media of embodiment 15, wherein the depth load filter layer comprises a high efficiency meltblown filter layer.
[0152] Embodiment 23 is the filter media of embodiment 22, wherein the high efficiency meltblown filter layer comprises meltblown fibers comprising polypropylene, polybutylene terephthalate, or a combination thereof.
[0153] Embodiment 24 is the filter media of embodiment 22 or 23, wherein the high efficiency meltblown filter layer comprises meltblown fibers having an average diameter between 0.5 microns and 10 microns.
[0154] Embodiment 25 is the filter media of embodiment 24, wherein the high efficiency meltblown filter layer comprises meltblown fibers having an average diameter between 0.5 microns and 4 microns.
[0155] Embodiment 26 is the filter media of embodiment 25, wherein the high efficiency meltblown filter layer comprises meltblown fibers having an average diameter between 1 micron and 3 microns.
[0156] Embodiment 27 is the filter media of embodiment 25, wherein the high efficiency meltblown filter layer comprises meltblown fibers having an average diameter between 2 microns and 3 microns.
[0157] Embodiment 28 is the filter media of any one of embodiments 1-27, wherein the depth loading filter layer exhibits a DEHS filtration efficiency of at least 55%.
[0158] Embodiment 29 is the filter media of embodiment 28, wherein the depth loading filter layer exhibits a DEHS filtration efficiency of at least 70%.
[0159] Embodiment 30 is the filter media of any one of embodiments 1-29, wherein the depth loading filter layer exhibits a DEHS filtration efficiency of up to 99.997%.
[0160] Embodiment 31 is the filter media of embodiment 30, wherein the depth loading filter layer exhibits a DEHS filtration efficiency of up to 99.97%.
[0161] Embodiment 32 is the filter media of embodiment 31, wherein the depth loading filter layer exhibits a DEHS filtration efficiency of up to 99.5%.
[0162] In embodiment 33, the deep load filter layer is up to 150 g / m 2 33. The filter media of any one of embodiments 1-32, having a basis weight of
[0163] Embodiment 34 is a method for manufacturing a depth load filter layer having a thickness of at least 10 g / m 2 The filter media of any one of embodiments 1 to 33, having a basis weight of
[0164] Embodiment 35 is a method for manufacturing a depth-loaded filter layer having a filtration rate of at least 1 g / m2 at a pressure increase of 500 Pascals relative to the initial value. 2 35. The filter medium of any one of embodiments 1 to 34, which exhibits a salt loading capacity of 100%.
[0165] In embodiment 36, the deep load filter layer has a maximum of 10 g / m2 at a pressure increase of 500 Pascals relative to the initial value. 2 The filter medium according to any one of the first to thirty-five embodiments, which exhibits a salt loading capacity of 100% or more.
[0166] Embodiment 37 is the filter media of any one of embodiments 1 to 36, wherein the support layer has a Gurley stiffness of 1000 milligrams or greater.
[0167] In embodiment 38, the support layer is at least 10 ft 3 / min (80.2 l / m at 200 Pa) 2 28. The filter media of embodiment 27 having a permeability of 100 / sec.
[0168] Embodiment 39 is the filter media of any one of embodiments 1-38, wherein the support layer comprises wetlaid fibers.
[0169] Embodiment 40 is the filter media of embodiment 39, wherein the wetlaid fibers comprise cellulose, polyester, or a combination thereof.
[0170] In embodiment 41, the support layer is up to 260 g / m 2 The filter media of any one of embodiments 1 to 40, having a basis weight of
[0171] In embodiment 42, the support layer is at least 50 g / m 2 The filter media of any one of embodiments 1 to 41, having a basis weight of
[0172] Embodiment 43 is the filter media of any one of embodiments 1-42, further comprising a scrim layer disposed between the surface-loaded filter layer and the depth-loaded filter layer.
[0173] Embodiment 44 is the filter media of any one of embodiments 1-43 having a thickness of at least 10 mils (0.25 mm).
[0174] Embodiment 45 is the filter media of any one of embodiments 1-44, having a thickness of up to 60 mils (1.5 mm).
[0175] Embodiment 46 is the filter media of embodiment 45 having a thickness of up to 30 mils (0.76 mm).
[0176] Embodiment 47 is the filter media of any one of embodiments 1-46, wherein the layers are bonded together with adhesives, binder fibers, thermal bonds, ultrasonic bonds, self-adhesives, or combinations thereof.
[0177] Embodiment 48 is the filter media of any one of embodiments 1-47, exhibiting an efficiency of at least F9 according to EN779:2012.
[0178] Embodiment 49 is the filter media of embodiment 48, exhibiting at least 80%, or greater than 80%, efficiency according to the DEHS efficiency test at maximum penetrating particle size.
[0179] Embodiment 50 is the filter media of any one of embodiments 1-49 which is an air filter media.
[0180] A fifty-first embodiment is a gas filter element including a housing and the gas filter media of any one of the first to fifty embodiments.
[0181] Embodiment 52 is the gas filter element of embodiment 51, exhibiting an efficiency of at least F9 according to EN779:2012.
[0182] Embodiment 53 is the gas filter element of embodiment 52, exhibiting an efficiency of at least E10 according to EN1822:2009.
[0183] Embodiment 54 is the gas filter element of embodiment 53, exhibiting an efficiency of at least E11 according to EN1822:2009.
[0184] Embodiment 55 is the gas filter element of embodiment 54, exhibiting an efficiency of at least E12 according to EN1822:2009.
[0185] Embodiment 56 is the gas filter element of any one of embodiments 51-55, which is a flat panel, a cylindrical shape, or a conical shape.
[0186] Embodiment 57 is the gas filter element of any one of Embodiments 51-56, which is pleated.
[0187] Embodiment 58 is a method of filtering a gas (eg, air) comprising directing the gas through the filter of any one of embodiments 51-57.
[0188] Embodiment 59 is a method of filtering a gas comprising directing the gas through the filter medium of any one of embodiments 1-55. EXAMPLES
[0189] Objects and advantages of this disclosure are further illustrated by the following examples, in which the particular materials and amounts thereof recited, as well as other conditions and details, should not be construed to unduly limit this disclosure.
[0190] Test Method Salt tolerance test 20 mg / m 3 of NaCl salt particles (0.33 μm mass median diameter) in 100 cm of filtration media. 2A TSI8130 bench was used to load the samples. The flow rate on the bench was chosen to represent real world conditions. Other settings for the bench are such that they are driven to manufacturer specifications. The media is loaded with anywhere from 4" to 10" H2O (1000-2500 Pa) of dP before the end of the test, depending on the requester's needs. Every minute, the bench measures the amount of salt loaded, salt passed through, and dP across the media. This data is recorded by the bench. Before and after the test is completed, the samples are weighed and the difference in weight is the salt loaded, and this value is used to calibrate the photometer.
[0191] 0.5 g / ft when loaded to a 2 in. H2O pressure drop rise at a media velocity of 10 feet per minute (fpm) (5.33 cm / sec) 2 (5.38g / m 2 ) media having a larger carrying capacity is known to be a deep load media.
[0192] Modified ISO 11057 test method for the filtration characteristics of washable filter materials To determine the pulse-cleaning ability of the filter media, a modified version of the ISO 11057 test method for the filtration characteristics of washable filter media was used. The ISO standard has five stages. Stage 2 of the test was used with the following modifications: Primary stroke flow speed: 2.54m 3 / hr, Secondary stroke flow speed: 5.07m 3 / hr, Maximum limit 1800Pa, Dust feed rate: 2.0g / m 3 , Pulse strength: 0.1MPa, and Tested every 200 seconds for a total of 300 cycles. All other test conditions remain the same. The pressure drop (dP) of the media immediately after pulsing was recorded for each cycle. The final dP after 300 cycles and the extrapolated dP to 3000 cycles were used to compare the performance of the pulse-cleanable media. The extrapolation method was logarithmic or power equation (whichever was higher) with a R 2 This was done by performing a curve fit to the data (at 300 pulses) and then using that equation to determine dP at 3000 pulses.
[0193] DEHS Efficiency Test 100cm at flows representative of real world conditions 2 A TSI3160 bench was used to test the efficiency of the sample media, in this case a flow of 4 feet per minute (fpm) was used. A sprayer creates a distribution of DEHS droplets, and a Differential Mobility Analyzer (DMA) is used to classify the DEHS droplet distribution into a monodisperse cloud of particles. The droplet sizes for this test are 0.09, 0.1, 0.2, 0.3 and 0.4 μm. A Condensation Particle Counter (CPC) then measures the start-up concentration upstream and downstream of the filter sample to determine the media efficiency at that particle size. All other settings are to the manufacturer's specifications.
[0194] After the efficiency for all particle sizes has been determined, the system fits a curve to these points to determine which particle size is associated with the highest penetration (lowest efficiency), which is called the maximum penetrating particle size (MPPS), and can be the calculated penetration based on the fitted curve for that particular media sample.
[0195] LEFS Test A 4-inch diameter sample is cut from the media. The particle capture efficiency of the test specimen is calculated from 0.8 μm latex spheres as test induced contamination in a LEFS (see ASTM Standard F1215-89 for a description of LEFS testing) bench operating at 20 fpm.
[0196] Working Example Example 1 Laminated filter media was prepared using the following technique: A 50 gsm wet-laid filter material containing a mixture of glass and bicomponent PET fibers was prepared similar to that of Example 6 in U.S. Patent No. 7,314,497 (with the modification that it consisted of 40% B08 microglass fibers from Lauscha Fiber International (Lauscha, Germany) and 60% TJ04BN bicomponent PET fibers from Teijin (Osaka, Japan). A 116 gsm wet-laid media consisting of 90% cellulose and 10% polyester blend support material was purchased from H&V of East Walpole, MA. Sheet properties are in Table 1.
[0197] [Table 1]
[0198] The two rolls were layered with the glass bicomponent layer on top and the cellulose polyester blend on the bottom. EMS-Griltech granular adhesive from Switzerland (Griltex 9E) was applied at 4.07 g / m 2 was applied between the two layers which were then heat laminated at 265°F.
[0199] After lamination, a fine fiber layer was applied to the 50 gsm glass bicomponent layer, which was composed of 0.2-0.3 micron sized fibers and was made of nylon with a LEFS efficiency of 82.4%.
[0200] The laminated, nanofiber coated media was tested for its planar sheet properties and the elements were tested for dP and efficiency using the EN 1822 procedures. The results are shown in Table 2.
[0201] [Table 2]
[0202] The flat sheet media was pleated to a pleat depth of 2 inches (5.1 cm) and assembled into 26 inch (66 cm) conical and cylindrical filter pairs. The conical elements had 280 pleats per element, while the cylindrical elements had 230 pleats. The elements were made with the nanofiber layer facing upstream.
[0203] Example 2 Laminated filter media was prepared using the following technique: A 50 gsm wet-laid filter material containing a mixture of glass and bicomponent PET fibers was prepared similar to that of Example 6 in U.S. Patent No. 7,314,497 (with the modification that it consisted of 40% B08 microglass fibers from Lauscha Fiber International (Lauscha, Germany) and 60% TJ04BN bicomponent PET fibers from Teijin (Osaka, Japan). A 116 gsm wet-laid media consisting of 90% cellulose and 10% polyester blend support material was purchased from H&V of East Walpole, MA. Sheet properties are in Table 3.
[0204] [Table 3]
[0205] These two rolls were layered with the glass bicomponent layer on the upstream and the cellulose polyester blend on the bottom. The two layers were 4.07 g / m 2The laminated nanofiber coated media was heat laminated at 265°F using Griltex 9E, granular adhesive (EMS-Griltech, Switzerland) between each layer. After lamination, a fine fiber layer was applied to the 116 gsm wet-laid cellulose polyester blend layer. This fine fiber layer consisted of nylon fibers sized 0.2-0.3 microns with a LEFS efficiency of 78%. The laminated nanofiber coated media was tested for its planar sheet properties. The results are shown in Table 4.
[0206] [Table 4]
[0207] The flat sheet media was pleated to a pleat depth of 2 inches (5.1 cm) and assembled into 26 inch (66 cm) conical and cylindrical filter pairs. The conical elements had 250 pleats per element, while the cylindrical elements had 210 pleats. The elements were made with the nanofiber layer facing upstream.
[0208] Example 3 Laminated filter media was prepared using the following technique: A 50 gsm wet-laid filter material containing a mixture of glass and bicomponent fibers was prepared similar to that of Example 6 in U.S. Patent No. 7,314,497, with the modification that it consisted of 50% B08 microglass fiber from Lauscha Fiber International (Lauscha, Germany) and 50% bicomponent PET fiber (TJ04BN) from Teijin (Osaka, Japan). A 100 gsm spunbond support material of Finon C310NW was purchased from Midwest Filtration of Cincinnati, Ohio. Sheet properties are in Table 5.
[0209] [Table 5]
[0210] These two rolls were layered with the wet layer upstream and the spunbond layer downstream. 2 and heat laminated at 275° F. using granular adhesive Griltex 9E (EMS-Griltech, Switzerland) between each layer.
[0211] The material was then corrugated to an average depth of 0.027 inches (0.69 mm) (measured in the z-direction from the top of the peak to the bottom of the groove on the wire side of the media) at 4.5 corrugations per inch (1.77 corrugations / cm). After corrugation, a fine fiber layer was applied to the 50 gsm wet layer. This fine fiber layer was composed of nylon fibers sized 0.2 to 0.3 microns with a LEFS efficiency of 66%.
[0212] The laminated, corrugated and coated media was tested for its planar sheet properties and the results are shown in Table 6.
[0213] [Table 6]
[0214] The flat sheet media was pleated to a 2 inch (5.1 cm) pleat depth and assembled into a 26 inch (66 cm) conical and cylindrical filter pair. The conical elements had 210 pleats per element, while the cylindrical elements had 176 pleats per element. The elements were made with the nanofiber layer facing upstream.
[0215] Example 4 Laminated filter media was prepared using the following techniques: An 18.6 gsm spunbond scrim layer of FINON C3019 was purchased from Midwest Filteration, Cincinnati, OH. A 50 gsm wet-laid filter material containing a mixture of glass and bicomponent fibers was prepared similar to that of Example 6 in U.S. Pat. No. 7,314,497, with the modification that it consisted of 50% B08 microglass fiber from Lauscha Fiber International, Lauscha, Germany, and 50% bicomponent PET fiber (TJ04BN) from Teijin, Osaka, Japan. A 100 gsm spunbond support material of Finon C310NW was purchased from Midwest Filteration, Cincinnati, OH. Sheet properties are in Table 7.
[0216] [Table 7]
[0217] The three rolls were layered such that the scrim layer was upstream, the wet layer was in the middle, and the spunbond layer was downstream. 2 The laminate was heat laminated at 275°F using GRILTEX 9E granular adhesive (EMS-Griltech, Switzerland) between each layer.
[0218] The material was then corrugated to an average depth of 0.0248 inches (0.63 mm) (measured in the z-direction from the top of the peak to the bottom of the groove on the wire side of the media) at 4.5 corrugations per inch (1.77 corrugations / cm).
[0219] After corrugation, a fine fiber layer was applied to the 18.6 gsm spunbond scrim layer. The fine fiber layer consisted of nylon fibers sized 0.2-0.3 microns with a LEFS efficiency of 66%. The laminated, corrugated, and fine fiber coated media was tested for its flat sheet properties. The results are shown in Table 8.
[0220] [Table 8]
[0221] Example 5 Laminated filter media was prepared using the following technique: A 50 gsm wet filter material containing a mixture of glass and bicomponent fibers was prepared similar to that of Example 6 in U.S. Patent No. 7,314,497, with the modification that it consisted of 50% B04 microglass fiber from Lauscha Fiber International, Lauscha, Germany, and 50% bicomponent PET fiber (TJ04BN) from Teijin, Osaka, Japan. A 116 gsm corrugated cellulose support material was purchased from H&V, East Walpole, MA. Sheet properties are in Table 9.
[0222] [Table 9]
[0223] These two rolls were layered with the wet layer upstream and the cellulose wet layer downstream. 2 The laminate was heat laminated at 275°F using Griltex 9E granular adhesive (EMS-Griltech, Switzerland) between each layer.
[0224] After lamination, a fine fiber layer was applied to the 50 gsm wet layer. This fine fiber layer consisted of nylon fibers sized 0.2-0.3 microns with a LEFS efficiency of 74%.
[0225] The laminated, fine fiber coated media was tested for its planar sheet properties and the results are shown in Table 10.
[0226] [Table 10]
[0227] The flat sheet media was pleated to a pleat depth of 2 inches (5.1 cm) and assembled into a 26 inch (66 cm) cylindrical filter pair. The elements had 250 pleats per element. The elements were constructed with the nanofiber layer facing upstream.
[0228] Example 6 Laminated filter media was prepared using the following technique: A 50 gsm wet-laid filter material containing a mixture of glass and bicomponent PET fibers was prepared similar to that of Example 6 in U.S. Patent No. 7,314,497 (with the modification that it was composed of 40% B08 microglass fibers from Lauscha Fiber International (Lauscha, Germany) and 60% TJ04BN bicomponent PET fibers from Teijin (Osaka, Japan). A 114 gsm wet-laid media composed of glass, polyester, and resin support material was purchased from H&V of East Walpole, MA. Sheet properties are in Table 11.
[0229] [Table 11]
[0230] The EN933 material was corrugated to an average depth of 0.0283 inches (0.72 mm) (measured as the distance in the z-direction from the top of the peak to the bottom of the groove on the wire side of the media) with 4.5 corrugations per inch (1.77 corrugations / cm).
[0231] These two rolls were then laminated together with the glass bicomponent layer on the upstream and the glass polyester blend on the bottom. The two layers were 4.07 g / m 2 and heat laminated at 265°F using Griltex 9E, granular adhesive (EMS-Griltech, Switzerland) between each layer.
[0232] After lamination, a fine fiber layer was applied to the 50 gsm wet layer. This fine fiber layer consisted of nylon fibers sized 0.2-0.3 microns with a LEFS efficiency of 62.4%. The laminated, nanofiber coated media was tested for its planar sheet properties and the results are shown in Table 12.
[0233] [Table 12]
[0234] The flat sheet media was pleated to a pleat depth of 2 inches (5.1 cm) and assembled into 26 inch (66 cm) conical and cylindrical filter pairs. The conical elements had 266 pleats per element, while the cylindrical elements had 220 pleats per element. The elements were made with the nanofiber layer facing upstream.
[0235] The complete disclosures of the patents, patent documents, and publications cited herein are incorporated by reference in their entirety as if each were separately incorporated. Various modifications and alterations to this disclosure will be apparent to those skilled in the art without departing from the scope and spirit of this disclosure. It should be understood that this disclosure is not intended to be unduly limited by the exemplary embodiments and examples described herein, and that such examples and embodiments are presented by way of example only, and that the scope of this disclosure is intended to be limited only by the claims set forth herein below.
Claims
1. 1. A gas filter medium comprising: a surface-loaded filter layer comprising fine fibers having an average diameter of less than 1 micron; a depth-loading filter layer comprising a glass-containing filter layer comprising glass fibers and multicomponent binder fibers, said depth-loading filter layer exhibiting a DEHS filtration efficiency of at least 55% when measured at 2 cm / sec for 0.4 μm particles; With supporters Includes 13. A gas filter media, wherein the layers are constructed and arranged for placement in a gas stream with the surface-loaded filter layer being the most upstream layer, the gas filter media having a thickness of 0.25 mm to 0.76 mm.
2. 10. The filter media of claim 1, wherein the depth-loading filter layer is positioned between the surface-loading filter layer and the support layer.
3. 3. The filter media of claim 1 or 2, wherein the fine fibers have an average diameter of at least 0.01 microns and at most 0.5 microns.
Citation Information
Patent Citations
Filter media and structures
JP2008518772A
Corrugated filter material and filter element
JP2010520049A
Cleanable high efficiency filter media structure and applications for use
US20040255783A1
Dust filter bag containing nano non-woven tissue
US6395046B1