High-strength austenitic stainless steel with improved low-temperature toughness in hydrogen environments

Austenitic stainless steel with controlled alloy composition and microstructure addresses low-temperature toughness and hydrogen embrittlement issues, ensuring high strength and impact toughness for hydrogen storage applications.

JP7591146B2Active Publication Date: 2024-11-27POHANG IRON & STEEL CO LTD
View PDF -1 Cites 0 Cited by

Patent Information

Application Number
JP2023530923
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-11-23
Filing Date
2021-11-01
Publication Date
2024-11-27
Estimated Expiration
2041-11-01

AI Technical Summary

Technical Problem

Existing austenitic stainless steels used in hydrogen environments suffer from decreased toughness at low temperatures and hydrogen embrittlement, which is critical for applications in fuel cell vehicles and hydrogen storage containers.

Method used

Austenitic stainless steel with controlled alloy composition (C: 0.1% or less, Si: 1.5% or less, Mn: 0.5~3.5%, Cr: 17~23%, Ni: 8~14%, N: 0.15~0.3%, Mo: 2% or less, Cu: 0.2~2.5%, Nb: 0.05% or less, V: 0.05% or less) and microstructure with precipitates <100 μm², ensuring high strength and improved low-temperature toughness.

Benefits of technology

The steel exhibits yield strength of 300 MPa or more at room temperature and Charpy impact energy of 100 J or more at -196°C, with minimal hydrogen embrittlement, maintaining high impact toughness in hydrogen environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007591146000001
    Figure 0007591146000001
  • Figure 0007591146000002
    Figure 0007591146000002
  • Figure 0007591146000003
    Figure 0007591146000003
Patent Text Reader

Abstract

The present invention relates to a high-strength austenitic stainless steel having improved low-temperature toughness in a hydrogen environment. [Solution] The austenitic stainless steel of the present invention, which has improved low-temperature toughness in a hydrogen environment, is composed of, by weight, C: 0.1% or less, Si: 1.5% or less, Mn: 0.5-3.5%, Cr: 17-23%, Ni: 8-14%, N: 0.15-0.3%, the remainder being Fe and impurities, and optionally further containing at least one of Mo: 2% or less, Cu: 0.2-2.5%, Nb: 0.05% or less, and V: 0.05% or less, and the microstructure contains precipitates with an average diameter of 30-1000 nm or less, with a density of 100 μm or less. 2 They are distributed in numbers of less than 20 per unit area.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a high-strength austenitic stainless steel having improved low-temperature toughness in a hydrogen environment. [Background technology]

[0002] In recent years, greenhouse gases (CO2, NO X , S.O. X In order to reduce CO2 emissions, the development and spread of fuel cell vehicles that use hydrogen as fuel is expanding. This has created a need to develop materials that can be used as hydrogen storage containers and parts.

[0003] Hydrogen storage containers can be divided into liquefied hydrogen storage containers and gaseous hydrogen storage containers depending on the state of hydrogen. In particular, liquefied hydrogen storage methods have higher storage efficiency than gaseous hydrogen storage methods, and will be used in various fields in the future. For example, liquefied hydrogen storage methods will be used for long-distance transportation of hydrogen from overseas to domestic locations, and as a method for storing large amounts of hydrogen at hydrogen filling stations and hydrogen production plants.

[0004] The temperature at which hydrogen is used varies depending on its state, and gaseous hydrogen can generally be stored at room temperature, but it is cooled to about -40 to -60°C before filling the storage tank. This is to prevent an excessive rise in temperature due to filling, by cooling the gaseous hydrogen through a precooler, in consideration of the rise in gas temperature during filling.

[0005] Liquefied hydrogen is stored in an extremely low temperature environment of -253℃. Furthermore, in equipment that vaporizes liquefied hydrogen, steel is exposed to temperatures ranging from -253℃ to room temperature. Therefore, when considering the steel material for hydrogen storage tanks, the deterioration of the physical properties of steel material due to hydrogen not only at room temperature but also at extremely low temperatures becomes an important factor in the crystallization of steel material.

[0006] Meanwhile, in order to popularize and develop a hydrogen energy society centered on fuel cell vehicles in the future, it is essential to reduce the costs of fuel cell vehicles and hydrogen stations by downsizing various devices. In other words, the amount of steel used in hydrogen environments must be reduced. For this reason, steel used in hydrogen environments is required to have even higher mechanical strength and corrosion resistance.

[0007] Currently, the materials commonly used in hydrogen gas and liquefied hydrogen environments are austenitic stainless steels 304L and 316L. The physical properties of these steels tend to decrease as the temperature decreases. In particular, the decrease in toughness is a problem that mainly appears at low temperatures. In addition, when exposed to a hydrogen environment, hydrogen penetrates into the steel, causing further deterioration of the steel's physical properties due to hydrogen. Therefore, the deterioration of physical properties due to temperature and hydrogen must be judged simultaneously. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] Korean Patent Publication No. 10-2013-0067007 Summary of the Invention [Problem to be solved by the invention]

[0009] The present invention aims to provide a high-strength austenitic stainless steel that ensures high impact toughness at cryogenic temperatures through control of the alloy composition and has improved low-temperature toughness in a hydrogen environment. [Means for solving the problem]

[0010] The austenitic stainless steel of the present invention is composed of, by weight percent, C: 0.1% or less, Si: 1.5% or less, Mn: 0.5 to 3.5%, Cr: 17 to 23%, Ni: 8 to 14%, N: 0.15 to 0.3% or less, the remainder being Fe and impurities, and optionally further containing at least one of Mo: 2% or less, Cu: 0.2 to 2.5%, Nb: 0.05% or less, and V: 0.05% or less, and has a microstructure containing precipitates with an average diameter of 30 to 1000 nm or less and a diameter of 100 μm or less. 2 Win 1 pieces less than It is distributed in.

[0011] Furthermore, the austenitic stainless steel of the present invention can satisfy the yield strength at room temperature of 300 MPa or more.

[0012] Furthermore, the austenitic stainless steel of the present invention can satisfy a Charpy impact energy value of 100 J or more at −196° C., measured after hydrogen is charged into the steel material under conditions of 300° C. and 10 MPa.

[0013] In addition, the austenitic stainless steel of the present invention can satisfy the requirement that the difference between a first Charpy impact energy value measured without charging hydrogen at any temperature of -50°C or less and a second Charpy impact energy value measured after charging hydrogen under conditions of 300°C and 10 MPa is 30 J or less. Effect of the Invention

[0014] According to the present invention, a high-strength austenitic stainless steel having improved hydrogen embrittlement resistance can be provided. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] The austenitic stainless steel of the present invention is composed of, by weight percent, C: 0.1% or less, Si: 1.5% or less, Mn: 0.5 to 3.5%, Cr: 17 to 23%, Ni: 8 to 14%, N: 0.15 to 0.3% or less, the remainder being Fe and impurities, and optionally further containing at least one of Mo: 2% or less, Cu: 0.2 to 2.5%, Nb: 0.05% or less, and V: 0.05% or less, and has a microstructure containing precipitates with an average diameter of 30 to 1000 nm or less and a diameter of 100 μm or less. 2 Win 1 pieces less than It is distributed in.

[0016] Hereinafter, preferred embodiments of the present invention will be described. However, the embodiments of the present invention may be modified in various different forms, and the technical concept of the present invention is not limited to the embodiments described below. Furthermore, the embodiments of the present invention are provided to more completely explain the present invention to those having average knowledge in the art.

[0017] The terms used in this application are merely used to describe specific examples. Thus, for example, singular expressions include plural expressions unless the context clearly requires singularity. Furthermore, it should be noted that the terms "include" or "comprise" used in this application are used to clearly indicate the presence of features, steps, functions, components, or combinations thereof described in the specification, and are not used to preliminarily exclude the presence of other features, steps, functions, components, or combinations thereof.

[0018] On the other hand, unless otherwise defined, all terms used herein should be considered to have the same meaning as that generally understood by a person having ordinary knowledge in the technical field to which the present invention belongs. Therefore, unless clearly defined in this specification, a specific term should not be interpreted in an overly ideal or formal sense. For example, in this specification, a singular expression includes a plural expression unless there is a clear exception in the context.

[0019] In addition, in this specification, the terms "about," "substantially," and the like are used to mean a numerical value or a value close to that numerical value when the tolerances of manufacturing and materials inherent in the referred meaning are presented, and are used to prevent unscrupulous infringers from unfairly exploiting the disclosure content in which precise and absolute numerical values ​​are cited to aid in the understanding of the present invention.

[0020] Steels exposed to a hydrogen environment are likely to be exposed to a range of temperatures as well as the hydrogen environment, so temperature can be an important factor when applying steels to a hydrogen environment.

[0021] Generally, as the temperature decreases, the toughness of steel material decreases and brittleness appears. In particular, in a hydrogen atmosphere, not only does the temperature cause a decrease in physical properties, but hydrogen-induced brittleness can occur, which can cause major problems. Therefore, when selecting steel material to be used in a hydrogen environment, the effects of hydrogen and temperature must be evaluated simultaneously.

[0022] On the other hand, representative methods for increasing the strength of steel materials include a method using cold working and a method using precipitation strengthening due to precipitation.

[0023] However, the cold working method has a problem in that transformation of austenite to martensite occurs, and the transformed martensite may cause hydrogen embrittlement or a decrease in low temperature toughness.

[0024] The method using precipitation strengthening by precipitation has a problem that the precipitates cause a decrease in cryogenic toughness, and the improvement of strength by precipitation strengthening requires additional costs for the precipitate formation process.

[0025] Therefore, rather than improving strength by cold working or precipitation strengthening, it is necessary to develop materials with high stability of the austenitic structure and high strength through control of the alloy composition.

[0026] The present invention aims to provide a high-strength austenitic stainless steel having improved strength through solid solution strengthening by controlling the alloy composition of the steel, and improved low-temperature toughness in a hydrogen environment due to increased stability of austenite in the hydrogen environment.

[0027] A high-strength austenitic stainless steel with improved low-temperature toughness in a hydrogen environment according to one embodiment of the present invention comprises, by weight, C: 0.1% or less, Si: 1.5% or less, Mn: 0.5-3.5%, Cr: 17-23%, Ni: 8-14%, N: 0.15-0.3% or less, the remainder being Fe and impurities, and optionally further containing at least one of Mo: 2% or less, Cu: 0.2-2.5%, Nb: 0.05% or less, and V: 0.05% or less.

[0028] The reasons for limiting the chemical composition of the steel will be specifically explained below. Unless otherwise specified, the chemical compositions below are all expressed in weight percent.

[0029] Carbon (C): 0.1% or less C is an effective element for stabilizing the austenite phase, suppressing delta (δ) ferrite, and increasing strength through solid solution strengthening. However, excessive addition can induce grain boundary precipitation of Cr carbides, reducing ductility, toughness, corrosion resistance, etc. Therefore, it is preferable to control the C content range to 0.1% or less.

[0030] Silicon (Si): 1.5% or less Silicon is an effective element for improving corrosion resistance and solid solution strengthening. However, excessive addition of silicon not only promotes the formation of delta (δ) ferrite in the cast slab, lowering the hot workability of the steel material, but also lowering the ductility and toughness of the steel material. Therefore, it is preferable to control the content of silicon to 1.5% or less.

[0031] Manganese (Mn): 0.5-3.5% Mn is an element that stabilizes the austenite phase, suppressing the formation of processed martensite and improving cold rolling properties, so it is added at 0.5% or more. However, excessive addition of more than 3.5% increases sulfide inclusions (MnS), which may reduce the ductility, toughness, and corrosion resistance of the steel. Therefore, it is preferable to control the Mn content range to 0.5-3.5%.

[0032] Chromium (Cr): 17-23% Cr is added at 17% or more as an element necessary to ensure corrosion resistance. However, excessive addition of more than 23% may promote the formation of delta (δ) ferrite in the slab, which may reduce the hot workability of the steel. In addition, austenite becomes unstable, and a large amount of Ni must be included for phase stability, which may cause an increase in costs. Therefore, it is preferable to control the Cr content range to 17-23%.

[0033] Nickel (Ni): 8-14% Ni is added as an austenite phase stabilizing element to ensure low temperature toughness at 8% or more. However, Ni is an expensive element, and adding a large amount of it leads to an increase in raw material costs, so the upper limit is set at 14%. Therefore, it is preferable to control the Ni content range to 8-14%.

[0034] Nitrogen (N): 0.15-0.3% The more N is added, the more it stabilizes the austenite phase and improves the strength of the material, so 0.15% or more should be added. However, excessive addition of N reduces hot workability, so the upper limit is set at 0.3%. Therefore, it is preferable to control the N content range to 0.15-0.3%.

[0035] Molybdenum (Mo): 2% or less Mo is a ferrite stabilizing element that increases resistance to general corrosion and pitting corrosion in some acid solutions and improves the passive zone against corrosion of materials. However, excessive addition of Mo may promote the formation of delta (δ) ferrite, which may reduce the low-temperature toughness of steel. It also promotes the formation of sigma phase, which may reduce mechanical properties and corrosion resistance, so the upper limit is set at 2%. Therefore, it is preferable to control the Mo content range to 2% or less.

[0036] Copper (Cu): 0.2-2.5% Cu is an element that stabilizes the austenite phase and is effective in softening the material, so it is necessary to add 0.2% or more. However, Cu not only increases the cost of the material, but also forms a low melting point phase when added in excess, which reduces hot workability and quality. Therefore, the upper limit is set at 2.5%. Therefore, it is preferable to control the Cu content range to 0.2 to 2.5%.

[0037] Niobium (Nb), vanadium (V): 0.05% or less Nb and V are precipitation hardening elements that combine with carbon or nitrogen. The addition of these elements can suppress the formation of Cr precipitates that occur during cooling during cold rolling annealing. In addition, by suppressing the formation of Cr precipitates in the welded parts, it is possible to prevent a decrease in corrosion resistance.

[0038] However, if these elements are added in an amount exceeding 0.05%, they will crystallize as nitrides in the molten steel during casting, causing clogging of the casting nozzle and reducing the grain size, resulting in reduced hot workability. Therefore, it is preferable to control the Nb and V contents to 0.05% or less.

[0039] The remaining component of the present invention is iron (Fe). However, in a normal manufacturing process, unintended impurities may be inevitably mixed in from raw materials or the surrounding environment, and it is not possible to exclude these. Since any engineer of a normal manufacturing process would know about the impurities, the contents of all of them are not specifically mentioned in this specification.

[0040] In the austenitic stainless steel according to one embodiment of the present invention having the above-mentioned composition range, the precipitates having an average diameter of 30 to 1000 nm or less in the microstructure are 100 μm or less. 2 Win 1 pieces less than In the present invention, the precipitates refer to all precipitates that precipitate in steel, and include metal precipitates such as Cr, Nb, and V-based single precipitates or composite carbonitrides and Cu.

[0041] In addition, the austenitic stainless steel according to an embodiment of the present invention can satisfy a yield strength of 300 MPa or more at room temperature.

[0042] When an object is pulled with a certain amount of force and the force is released, it cannot return to its original state and becomes even longer. The maximum force at which it can return to its original state is called the yield strength. Increasing the strength of steel reduces the amount of steel used to manufacture a product of the same strength, which has the effect of reducing the cost of the product.

[0043] In addition, the austenitic stainless steel according to an embodiment of the present invention can satisfy a Charpy impact energy value of 100 J or more at -196°C or less, which is measured by charging hydrogen into the steel material under conditions of 300°C and 10 MPa.

[0044] The Charpy impact energy value is a value obtained through a Charpy impact test, in which a material is cut into a plate about 10 mm thick, a small notch is dug in the middle, the specimen is placed in a testing device, and impacts are applied with a hammer at different temperatures.

[0045] In addition, the austenitic stainless steel according to one embodiment of the present invention may satisfy the following: a difference of 30 J or less between a first Charpy impact energy value measured without charging hydrogen at any temperature of -50°C or less and a second Charpy impact energy value measured with charging hydrogen under conditions of 300°C and 10 MPa.

[0046] If the difference in Charpy impact energy between when hydrogen is charged and when it is not charged is 30 J or less, it is believed that there will be almost no deterioration in the material's physical properties due to hydrogen, and there will be no problems when using it in a hydrogen environment.

[0047] The present invention will be described in detail with reference to the following examples. However, the following examples are provided to illustrate and explain the present invention in more detail, and the scope of the present invention is not limited to these examples.

[0048] [Example] An austenitic slab having the composition shown in Table 1 below was hot rolled, and the hot-rolled steel sheet was annealed at a temperature of 900 to 1,200° C. The alloy composition of each of the examples and comparative examples is as shown in Table 1 below.

[0049] [Table 1]

[0050] Table 2 below shows Charpy impact energy values ​​without and with hydrogen charging for the examples and comparative examples. The Charpy impact energy values ​​were obtained through impact tests at room temperature (25°C), -50°C, -100°C, -150°C, and -196°C using ASTM E23 type A specimen standards. Hydrogen charging was performed by charging hydrogen into the steel at 300°C and a pressure of 10 MPa.

[0051] If the Charpy impact energy value at -196℃ is 100J or more, it can be considered to have improved cryogenic toughness. If the Charpy impact energy value at -196℃ is 100J or more even after hydrogen is charged, high impact toughness can be ensured even in a liquefied hydrogen environment.

[0052] [Table 2]

[0053] Example 1 13 and 15~Before hydrogen was charged, alloy 20 showed Charpy impact energy values ​​of 100 J or more at temperatures of 25°C, -50°C, -100°C, -150°C, and -196°C. Even after hydrogen was charged, alloy 20 showed values ​​of 100 J or more at all temperature ranges, demonstrating improved impact toughness at low and cryogenic temperatures.

[0054] On the other hand, Comparative Examples 2 to 4, in which hydrogen was charged at -196°C, showed Charpy impact energy values ​​of 100 J or less. This is because the degree of austenite stabilization was reduced due to the excessive addition of ferrite stabilizing elements. Comparative Examples 5 to 7, in which hydrogen was charged and in which hydrogen was not charged at -196°C, showed low Charpy impact energy values ​​of 100 J or less.

[0055] Table 3 below shows the difference in Charpy impact energy between the cases where hydrogen was not charged and where hydrogen was charged in the examples and comparative examples, and the difference in Charpy impact energy between the cases where hydrogen was charged and where hydrogen was charged at 100 μm. 2 are the number of precipitates per area and the yield strength.

[0056] The difference in Charpy impact energy between the presence and absence of hydrogen charging indicates the deterioration of the physical properties of the steel due to hydrogen. If the difference in Charpy impact energy is 30J or less, it can be considered that there is no deterioration of physical properties due to hydrogen.

[0057] The analysis of the deposits was carried out after collecting them using the replica extraction method. The replica extraction method involves first dissolving the matrix with an appropriate corrosive solution to slightly protrude the deposits and inclusions to create a replica, and then corroding the matrix again before peeling it off so that the deposits and inclusions adhere to the replica and fall off, which is then analyzed.

[0058] The number of precipitates was then counted using a transmission electron microscope (TEM). 2 The precipitates observed per area were measured, and the precipitates showed sizes of 30 to 1,000 nm.

[0059] [Table 3]

[0060] Example 1 13 and 15~ 20 has a high strength of 300 MPa or more, and the precipitates in the microstructure have an average diameter of 30 to 1000 nm or less and are 100 μm or less. 2 Per area 1 pieces less than In addition, the difference between the Charpy impact energy measured without hydrogen charging and the Charpy impact energy measured after hydrogen charging was 30 J or less in all temperature ranges.

[0061] On the other hand, in Comparative Example 1, the austenitic structure was unstable, and the difference between the Charpy impact energy measured without hydrogen charging and the Charpy impact energy measured after hydrogen charging exceeded 30 J in all temperature ranges. In addition, Comparative Example 1 had a low yield strength of 300 MPa or less, which shows that it is not suitable as a material for hydrogen.

[0062] In Comparative Examples 5 to 7, the precipitates were 100 μm. 2 Per area 1 This exceeded the limit, and a strength of 300 MPa or more was secured. However, looking at Table 2, both the cases with and without hydrogen charging at -196°C have low Charpy impact energy values ​​of 100 J or less. This is because the method of improving strength by using precipitates leads to a decrease in toughness in a low-temperature environment.

[0063] Although the exemplary embodiments of the present invention have been described above, the present invention is not limited thereto, and a person having ordinary knowledge in the art can understand that various changes and modifications are possible without departing from the concept and scope of the claims set forth below. [Industrial Applicability]

[0064] INDUSTRIAL APPLICABILITY The austenitic stainless steel according to the present invention has high impact toughness at cryogenic temperatures and has improved low-temperature toughness in a hydrogen environment, and therefore can be used as a material for hydrogen gas and liquefied hydrogen environments and has industrial applicability.

Claims

1. In weight percent, C: 0.1% or less, Si: 1.5% or less, Mn: 0.5-3.5%, Cr: 17-23%, Ni: 8-14%, N: 0.15-0.3% or less, the balance being Fe and impurities, and selectively further containing at least one of Mo: 2% or less, Cu: 0.2-2.5%, Nb: 0.05% or less, and V: 0.05% or less; The precipitates in the microstructure have an average diameter of 30 to 1000 nm or less and are 100 μm 2 1. An austenitic stainless steel having improved low temperature toughness in a hydrogen environment, characterized in that the number of lattice fractures is less than one per hydrogen atom.

2. 2. The austenitic stainless steel having improved low-temperature toughness in a hydrogen environment according to claim 1, characterized in that it has a yield strength of 300 MPa or more at room temperature.

3. 2. An austenitic stainless steel having improved low-temperature toughness in a hydrogen environment according to claim 1, characterized in that the Charpy impact energy value at -196°C measured by charging hydrogen into the steel material under conditions of 300°C and 10 MPa is 100 J or more.

4. 2. An austenitic stainless steel having improved low-temperature toughness in a hydrogen environment according to claim 1, characterized in that the difference between a first Charpy impact energy value measured without charging hydrogen at any temperature of -50°C or less and a second Charpy impact energy value measured with charging hydrogen under conditions of 300°C and 10 MPa is 30 J or less.