Semiconductor film and composite substrate
By controlling the off-angle distribution and biaxial orientation of ε-Ga2O3 films, the cracking issue is mitigated, enhancing the film's integrity and suitability for high-frequency HEMT devices.
Patent Information
- Application Number
- JP2023542234
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-08-20
- Filing Date
- 2022-06-09
- Publication Date
- 2024-11-27
- Estimated Expiration
- 2042-06-09
AI Technical Summary
Conventional ε-Ga2O3 semiconductor films frequently crack, hindering the production of high-quality power devices due to non-uniform film growth and misalignment of crystal orientations.
A semiconductor film with a controlled off-angle distribution of 0.25° or less and a maximum off-angle difference of 0.5° across specific points on the surface, combined with a biaxial orientation and a circular shape, to suppress crack generation and enhance film quality.
The solution effectively reduces crack formation and improves the integrity of ε-Ga2O3 films, enabling their application in high-frequency HEMT devices by maintaining a low crack density and ensuring uniform crystal orientation.
Smart Images

Figure 0007591154000003 
Figure 0007591154000004 
Figure 0007591154000005
Abstract
Description
[Technical field]
[0001] The present invention relates to an ε-Ga2O3-based semiconductor film and a composite substrate including the same. [Background technology]
[0002] In recent years, electronic devices (compound semiconductor devices) in which a GaN layer and an AlGaN layer are sequentially formed on a substrate and the GaN layer is used as an electron transport layer have been actively developed. One such compound semiconductor device is, for example, a GaN-based high electron mobility transistor (HEMT). By using a GaN-based HEMT as a switch of a power supply inverter, it is expected that both a reduction in on-resistance and an improvement in breakdown voltage can be achieved. However, when manufacturing a GaN-based HEMT, it is difficult to obtain a GaN substrate with high crystallinity, and thus there are various problems such as not being able to obtain high-frequency characteristics sufficient for practical use.
[0003] On the other hand, gallium oxide (Ga2O3) has attracted attention as a semiconductor material with a wider band gap than GaN. Gallium oxide (Ga2O3) is a transparent semiconductor with a wide band gap of 4.8-5.3 eV at room temperature, and absorbs almost no visible or ultraviolet light. Therefore, it is a promising material for use in optoelectronic devices and transparent electronics that operate in the deep ultraviolet region, and in recent years, photodetectors, light-emitting diodes (LEDs) and transistors based on gallium oxide (Ga2O3) have been developed. It is known that gallium oxide (Ga2O3) has five crystal structures: α, β, γ, σ and ε.
[0004] Although electronic devices using gallium oxide as a semiconductor have been investigated, Ga2O3, which has an α or β crystal structure, does not exhibit spontaneous polarization as a crystal structure, so its use as a semiconductor for HEMTs has not necessarily been suitable.
[0005] Meanwhile, in recent years, ε-Ga2O3 has also been studied. ε-Ga2O3 has a band gap of about 5 eV, is sufficiently stable up to about 870℃, and allows band gap control by forming mixed crystals. In addition, the generation of two-dimensional electron gas is required for application to HEMTs, and ε-Ga2O3 has a crystal structure that exhibits spontaneous polarization, making it more suitable as a semiconductor for HEMTs than α-Ga2O3 or β-Ga2O3.
[0006] For example, Patent Document 1 (JP Patent No. 6436538) discloses a low-impurity ε-Ga2O3 single crystal that is applicable to semiconductor elements and is produced using the HVPE (halide vapor phase epitaxy) method. Patent Document 2 (JP Patent Publication No. 2019-46984) discloses a method for manufacturing a semiconductor device with excellent semiconductor characteristics by forming, by a mist CVD method, a first semiconductor film containing as its main component a semiconductor crystal having a metastable crystal structure, and a second semiconductor film (mainly ε-Ga2O3) that has a different composition from the main component of the first semiconductor film and contains as its main component a semiconductor crystal having a hexagonal crystal structure. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Patent No. 6436538 [Patent Document 2] JP 2019-46984 A [Non-patent literature]
[0008] [Non-Patent Document 1] Ildiko Cora et al., "The real structure of ε-Ga2O3 and its relation to κ-phase," CrystEngComm, 2017, 19, 1509-1516 [Non-Patent Document 2] F. Mezzadri, et al., "Crystal Structure and Ferroelectric Properties of ε-Ga2O3 Films Grown on (0001)-Sapphire," Inorg. Chem. 2016, 55, 12079-12084 Summary of the Invention
[0009] As mentioned above, ε-Ga2O3 has a crystal structure that generates spontaneous polarization and allows band gap control by forming mixed crystals, making it a promising semiconductor material. However, conventional ε-Ga2O3-based semiconductor films frequently crack, which has been an obstacle to the fabrication of power devices.
[0010] The present inventors have now discovered that it is possible to suppress the occurrence of cracks in an ε-Ga2O3-based semiconductor film by controlling the off-angle distribution of the ε-Ga2O3-based semiconductor film.
[0011] SUMMARY OF THE PRESENT EMBODIMENT An object of the present invention is to provide an ε-Ga2O3-based semiconductor film in which the occurrence of cracks is suppressed.
[0012] According to the present invention, the following aspects are provided. [Aspect 1] A circular semiconductor film having a main phase of a crystal composed of ε-Ga2O3 or an ε-Ga2O3-based solid solution, The off-angle distribution on the surface of the semiconductor film is 0.25° or less, and the off-angle distribution is a maximum value θ of the off-angle at a center point X and four outer periphery points A, B, C, and D on the surface of the semiconductor film. max and the minimum value θ minthe off angle is defined as an inclination angle of a crystal axis oriented in a direction approximately normal to the semiconductor film with respect to a normal to the film surface of the semiconductor film, and the outer periphery points A, B, C, and D are determined such that i) a straight line connecting the outer periphery points A and C and a straight line connecting the outer periphery points B and D intersect at a right angle at the center point X, and ii) the shortest distance from the outer edge of the semiconductor film to each of the outer periphery points A, B, C, and D is 1 / 5 of the radius of the semiconductor film, When observing the entire surface of the semiconductor film excluding an area within 2 mm from the periphery, 2 A semiconductor film having 20 or fewer cracks each having a length of 50 μm or more, provided that a crack is considered to be one crack if the shortest distance between the cracks is 500 μm or less. [Aspect 2] 2. The semiconductor film according to aspect 1, wherein the semiconductor film has a surface with an arithmetic mean roughness Ra of 0.1 to 50 nm. [Aspect 3] 3. The semiconductor film according to aspect 1 or 2, wherein the arithmetic mean angle of the off angles at the center point X and the peripheral points A, B, C and D is 0.01 to 0.5°. [Aspect 4] 4. The semiconductor film according to any one of aspects 1 to 3, wherein the off-angle distribution is 0.15° or less. [Aspect 5] 5. The semiconductor film according to any one of aspects 1 to 4, wherein the thickness of the semiconductor film is 200 nm or more. [Aspect 6] A composite substrate having a two-layer structure composed of a GaN single crystal substrate and the semiconductor film according to any one of aspects 1 to 5 formed on the GaN single crystal substrate. [Brief description of the drawings]
[0013] [Figure 1] 1 is a diagram for explaining an off-angle on the surface of a semiconductor film according to the present invention; [Diagram 2] FIG. 2 is a diagram for explaining the positions of a center point X and four outer periphery points A, B, C and D on the surface of a semiconductor film of the present invention. [Diagram 3]FIG. 1 is a schematic cross-sectional view showing the configuration of an HVPE (halide vapor phase epitaxy) apparatus. [Figure 4] FIG. 1 is a schematic cross-sectional view showing the configuration of a mist CVD (chemical vapor deposition) apparatus. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] Semiconductor Film The semiconductor film according to the present invention has a crystal composed of ε-Ga2O3 or an ε-Ga2O3-based solid solution as a main phase. Therefore, the semiconductor film according to the present invention can be called an ε-Ga2O3-based semiconductor film. This semiconductor film has a circular shape, and therefore can be used as a semiconductor wafer. The off-angle distribution on the surface of the semiconductor film is 0.25° or less, and the off-angle distribution is determined by the maximum off-angle θ at the center point X and each of the four outer periphery points A, B, C, and D of the surface of the semiconductor film. max and the minimum value θ min The off angle is defined herein as the inclination angle θ of the crystal axis T oriented in the direction approximately normal to the semiconductor film 10 with respect to the normal N to the film surface of the semiconductor film 10, as shown in FIG. 1. The outer periphery points A, B, C, and D are determined as shown in FIG. 2 such that i) a straight line connecting the outer periphery points A and C and a straight line connecting the outer periphery points B and D intersect at a right angle at the center point X, and ii) the shortest distance from the outer edge of the semiconductor film to each of the outer periphery points A, B, C, and D is 1 / 5 of the radius of the semiconductor film. The inventors have determined the maximum value θ of the off angle of the semiconductor film at five such points sufficiently separated from each other. max and the minimum value θ min It has been found that by making the difference between the angle θ and the surface roughness θ of the semiconductor film 0.25° or less, it is possible to suppress the occurrence of cracks over a wide range from the center to the outer periphery of the semiconductor film. The semiconductor film according to the present invention has a surface roughness of 0.25° or less over a unit area of 20 cm when observed over the entire film surface excluding an area within 2 mm from the outer periphery of the semiconductor film (typically the outer periphery of the base substrate). 2 The number of cracks with a length of 50 μm or more per unit area is 20 or less. However, in this case, if the shortest distance from one crack to another is 500 μm or less, the cracks are considered to be one crack.
[0015] As mentioned above, ε-Ga2O3 has a higher possibility of being applied to HEMT devices than α-Ga2O3 or β-Ga2O3. This is because, while application to HEMT devices requires the generation of two-dimensional electron gas, ε-Ga2O3 has a crystal structure that generates spontaneous polarization and has the characteristic that band gap control is possible by forming a mixed crystal. However, conventional ε-Ga2O3-based semiconductor films have a high frequency of cracking, which is an obstacle to the fabrication of power devices. In this regard, the semiconductor film of the present invention can conveniently solve these problems.
[0016] The semiconductor film of the present invention has a surface area of 20 cm2 when observed from the entire surface of the film excluding a region within 2 mm from the outer periphery of the semiconductor film. 2 The number of cracks having a length of 50 μm or more per unit area is 20 or less. The number of cracks is preferably 20 or less, and more preferably 10 or less. The fewer the cracks, the better, and there is no particular lower limit to the number of cracks, but ideally it is 0, and typically it is 1 or more.
[0017] The semiconductor film of the present invention has a maximum off-angle θ at the center point X and each of the four outer periphery points A, B, C, and D on its surface. max and the minimum value θ min The off-angle distribution, which is the difference between the above values, is 0.25° or less, preferably 0.15° or less, and more preferably 0.10° or less. Since the off-angle distribution is preferably small, the lower limit is not particularly limited, and is ideally 0°, but typically 0.01° or more. In addition, on the surface of the semiconductor film, the arithmetic mean angle of the off-angles at the center point X and the peripheral points A, B, C, and D is preferably 0.01 to 0.5°, more preferably 0.05 to 0.45°, and further preferably 0.1 to 0.4°.
[0018] The measurement of the off-angle can be carried out by a known method. For example, the off-angle can be measured by using an automatic X-ray crystal orientation measurement device (FSAS III, manufactured by Rigaku) with a sampling width of 0.01° and a scan speed of 10° / min. In the present invention, the off-angles at a total of five points, namely, the center point X and four outer peripheral points A, B, C, and D on the surface of the semiconductor film, are used as representative values. This is because, when evaluating the off-angle distribution, it takes time to evaluate the entire surface of the semiconductor film and is not practical.
[0019] As described above, the semiconductor film of the present invention has a crystal composed of ε-Ga2O3 or ε-Ga2O3-based solid solution as a main phase. In this specification, "having a crystal composed of ε-Ga2O3 or ε-Ga2O3-based solid solution as a main phase" means that the crystal composed of ε-Ga2O3 or ε-Ga2O3-based solid solution occupies 80% by weight or more of the semiconductor film, preferably 90% by weight or more, more preferably 95% by weight or more, even more preferably 97% by weight or more, particularly preferably 99% by weight or more, and most preferably 100% by weight. The ε-Ga2O3-based solid solution is a solid solution of ε-Ga2O3 with other components. For example, the semiconductor film of the present invention can be composed of an ε-Ga2O3-based solid solution in which one or more components selected from the group consisting of Cr2O3, Fe2O3, Ti2O3, V2O3, Ir2O3, Rh2O3, In2O3, and Al2O3 are solid-solved in ε-Ga2O3. In addition, by dissolving these components in solid solution, it becomes possible to control the band gap, electrical properties, and / or lattice constant of the semiconductor film. The amount of these components dissolved in solid solution can be appropriately changed according to the desired properties. In addition, the ε-Ga2O3 solid solution may contain other components such as Si, Sn, Ge, N, Mg, etc. as dopants.
[0020] However, the crystal structure of ε-Ga2O3 has not been fully elucidated at the current technical level, and it is possible that what is identified as κ-Ga2O3 in crystal structure analysis may also be identified as ε-Ga2O3, or what is identified as ε-Ga2O3 may also be identified as κ-Ga2O3. For example, Non-Patent Document 1 (Ildiko Cora et al., "The real structure of ε-Ga2O3 and its relation to κ-phase," CrystEngComm, 2017, 19, 1509-1516) suggests that the crystal structure of ε-Ga2O3 (hexagonal crystal) and the crystal structure of κ-Ga2O3 (rectangular crystal) may be confused depending on the resolution of the probe technology. Therefore, in this specification, the term "ε-Ga2O3" refers not only to ε-Ga2O3 but also to κ-Ga2O3. That is, in this specification, even if it is identified as having the crystal structure of κ-Ga2O3, it is considered to be "ε-Ga2O3" and is included in the term "ε-Ga2O3".
[0021] The orientation direction of the ε-Ga2O3-based semiconductor film of the present invention in the approximately normal direction is not particularly limited, but is preferably c-axis orientation. However, a typical ε-Ga2O3-based semiconductor film is composed of ε-Ga2O3 or a mixed crystal of ε-Ga2O3 and a different material, and is oriented in two axes, the c-axis and the a-axis. As long as it is oriented in two axes, the ε-Ga2O3-based semiconductor film may be a mosaic crystal. A mosaic crystal is a collection of crystals that do not have clear grain boundaries, but whose orientation orientations are slightly different in one or both of the c-axis and the a-axis. The method for evaluating the biaxial orientation is not particularly limited, but known analytical methods such as EBSD (Electron Back Scatter Diffraction Patterns) method and X-ray pole figures can be used. For example, when the EBSD method is used, inverse pole figure mapping of the surface (film surface) of the biaxially oriented ε-Ga2O3 film or a cross section perpendicular to the film surface is measured. In the obtained inverse pole figure mapping, when two conditions are satisfied, namely (A) the film surface is oriented in a specific direction, and (B) the film surface is oriented in an axis perpendicular to the orientation direction of the approximately normal direction in a direction perpendicular to the normal direction, the film surface can be defined as being oriented in two axes, the approximately normal direction and the approximately film surface direction. In other words, when the above two conditions are satisfied, it is determined that the film surface is oriented in two axes, the c-axis and the a-axis. For example, when the approximately normal direction of the film surface is oriented in the c-axis, it is sufficient that the approximately film surface direction is oriented in a specific direction (e.g., the a-axis) perpendicular to the c-axis.
[0022] The semiconductor film of the present invention is circular, preferably with a diameter of 5.08 cm (2 inches) or more, and may be 10.0 cm or more. The upper limit of the size of the semiconductor film is not particularly limited, but is typically 30.0 cm or less in diameter, more typically 20.0 cm or less in diameter. In this specification, the "circular shape" does not necessarily mean a perfect circular shape, and may be a substantially circular shape that can be recognized as a circle as a whole. For example, a part of the circle may be cut out for specifying the crystal orientation or for other purposes. In this case, the outer edge shape of the semiconductor film considered when defining the center point X and the four outer periphery points A, B, C, and D may be determined based on the circular shape assumed when it is assumed that there is no cutout portion. Incidentally, the semiconductor film of the present invention is characterized by a small off-angle distribution, and the center point X and the outer periphery points A, B, C, and D are merely defined for convenience so that a representative off-angle value of the entire semiconductor film can be evaluated. Therefore, in order to uniquely determine the positions of the center point X and the outer periphery points A, B, C, and D, the shape of the semiconductor film is specified as a circle, but the essential meaning does not change even if the shape of the semiconductor film is not a circle. For example, even if the shape of the semiconductor film is a square or a rectangle (rectangle), it can be considered as an equivalent of the semiconductor film of the present invention as long as the off-angle distribution on the surface of the semiconductor film is small. In the semiconductor film of such a shape, the maximum circle inscribed in the outer periphery of the film when the square or rectangular semiconductor film is viewed from above is defined as a virtual circle, and the positions of the outer periphery points A, B, C, and D can be determined from the center point X of the virtual circle and the diameter of the virtual circle (similar to the case of the circular semiconductor film described above). By evaluating the off-angles at the center point X and the outer periphery points A, B, C, and D determined in this way, an evaluation similar to that of the circular semiconductor film can be performed.
[0023] By the way, the cause of the distribution of off-angles in the ε-Ga2O3-based semiconductor film is unclear, but it is thought to be formed for the following reasons. First, the existence of regions with different off-angles means that there are regions with slightly different orientations on the surface of the semiconductor film. The reason why the orientation of the ε-Ga2O3-based semiconductor film is shifted is unclear, but it is thought to be caused by the inhomogeneous film formation state when the semiconductor film is formed on the base substrate. Specifically, when the film formation conditions such as the substrate temperature, the raw material, and the amount of dopant supplied are inhomogeneous within the surface of the base substrate for film formation, or when the surface state of the base substrate for film formation is different within the surface, the growth behavior of the semiconductor film becomes inhomogeneous and the orientation orientation is shifted and the film grows. For example, i) if the heating rate during film formation is too fast, a temperature distribution is likely to occur in the base substrate. ii) If there is unevenness in the flow rate of the film formation gas or carrier gas within the surface of the base substrate for film formation, the growth behavior is likely to become inhomogeneous. iii) When a substrate having a large warp is used for film formation, the growth behavior may become non-uniform.
[0024] Regarding iii) above, if the base substrate is significantly warped, the base substrate will come into partial contact with a substrate holder such as a susceptor, which is likely to cause unevenness in the substrate temperature. In addition, warping generates stress on the surface of the base substrate for film formation, which results in non-uniform lattice constants. This is also considered to be one of the factors that cause non-uniform growth behavior. Even when a thin base substrate is used, warping is likely to occur during film formation. Examples of effective methods for suppressing warping during film formation include application of appropriate film formation conditions, use of a thick base substrate for film formation, and application of a support that suppresses warping.
[0025] The non-uniformity of the growth behavior of the semiconductor film as described above tends to become more pronounced as the substrate size increases. For example, the effect becomes greater as the substrate diameter becomes 5.08 cm (2 inches) or more, 10.0 cm (4 inches) or more, or 15.0 cm (6 inches) or more. In this regard, the semiconductor film of the present invention can be fabricated with a small off-angle distribution and suppressed crack generation even if the size of the base substrate is large (for example, 5.08 cm (2 inches) or more, 10.0 cm (4 inches) or more, or 15.0 cm (6 inches) or more).
[0026] By the way, by forming a Ga2O3 film on a GaN substrate, an ε-Ga2O3-based semiconductor film can be preferably produced. However, an ε-Ga2O3-based semiconductor film formed on a GaN substrate with a different lattice constant from ε-Ga2O3 may become an aggregate of domains (mosaic crystals) with very slightly different crystal orientations depending on the film formation conditions. The reason for this is unclear, but one possible reason is that the film formation temperature is relatively low because ε-Ga2O3 is in a metastable phase. Because the film formation temperature is low, it is difficult for adsorbed components to migrate on the substrate surface, making step-flow growth difficult. For this reason, the growth mode of island-like growth (three-dimensional growth) tends to be dominant. In particular, when the lattice mismatch between the ε-Ga2O3-based semiconductor film and the substrate for film formation is large, the crystal orientation orientations of the island-like growth parts (domains) may differ slightly. For this reason, each domain does not completely meet, and tends to become a mosaic crystal. It is possible that the accumulation of such microscopic differences in orientation may cause off-angle distribution. For this reason, it is preferable to suppress the mosaic effect by appropriately controlling the deposition conditions such as the deposition temperature, the raw material supply rate, etc. By appropriately selecting the deposition conditions in this way, the deviation in the orientation of the ε-Ga2O3-based semiconductor film is reduced, and as a result, an ε-Ga2O3-based semiconductor film with a small off-angle distribution can be realized.
[0027] The thickness of the semiconductor film of the present invention may be adjusted appropriately from the viewpoints of cost and required properties. That is, if the film is too thick, it takes a long time to form the film, so it is preferable that the film is not extremely thick from the viewpoint of cost. On the other hand, in order to improve the crystal quality, it is preferable to make the film relatively thick. In this way, the film thickness may be adjusted appropriately according to the desired properties.
[0028] The arithmetic mean roughness Ra of the surface of the semiconductor film of the present invention is preferably 0.1 to 50 nm, more preferably 0.1 to 30 nm, and further preferably 0.1 to 10 nm. The arithmetic mean roughness Ra may be measured in accordance with JIS B 0601 (2001).
[0029] The semiconductor film of the present invention may contain a Group 14 element as a dopant. Here, the Group 14 element refers to an element in Group 14 according to the periodic table established by IUPAC (International Union of Pure and Applied Chemistry), specifically, any one of carbon (C), silicon (Si), germanium (Ge), tin (Sn), and lead (Pb). The content of the dopant (Group 14 element) in the semiconductor film is preferably 1.0×10 15 ~1.0×10 21 / cm 3 , more preferably 1.0×10 17 ~1.0×10 19 / cm 3 It is preferable that these dopants are distributed homogeneously in the film, and that the dopant concentrations on the front and back surfaces of the semiconductor film are approximately the same.
[0030] The semiconductor film of the present invention may be in the form of a free-standing film of the film alone. Also, the semiconductor film formed on the base substrate for film formation may be separated and transferred to another support substrate. The material of the other support substrate is not particularly limited, but a suitable one may be selected from the viewpoint of material properties. For example, from the viewpoint of thermal conductivity, a metal substrate such as Cu, a ceramic substrate such as SiC or AlN, etc. are preferable. It is also preferable to use a substrate having a thermal expansion coefficient of 6 to 13 ppm / K at 25 to 400°C. By using a support substrate having such a thermal expansion coefficient, the thermal expansion difference with the semiconductor film can be reduced, and as a result, crack generation in the semiconductor film and film peeling due to thermal stress can be suppressed. An example of such a support substrate is a substrate made of a Cu-Mo composite metal. The composite ratio of Cu and Mo can be appropriately selected taking into consideration the thermal expansion coefficient matching with the semiconductor film, thermal conductivity, electrical conductivity, etc.
[0031] Method for manufacturing semiconductor film The semiconductor film of the present invention can be manufactured by forming a film of an ε-Ga2O3-based material on a GaN single crystal substrate, which is preferably used as a base substrate. The semiconductor layer can be formed by any known method, but preferred examples include mist CVD (mist chemical vapor deposition), HVPE (halide vapor phase epitaxy), MBE (molecular beam epitaxy), MOCVD (metal organic vapor phase epitaxy), and hydrothermal synthesis, with mist CVD or HVPE being particularly preferred. In the case of vapor phase epitaxy such as mist CVD or HVPE, the thickness of the base substrate is preferably 0.5 mm or more, more preferably 0.8 mm or more, and even more preferably 1.4 mm or more. With such a thickness, warping of the base substrate is unlikely to occur during film formation, and a semiconductor film with a small off-angle distribution can be easily formed. The upper limit of the thickness of the base substrate is not particularly limited, but is typically 5.0 mm or less, and more typically 4.0 mm or less.
[0032] The particularly preferred film formation methods, HVPE and mist CVD, will be described below.
[0033] The HVPE method (Halide Vapor Phase Epitaxy) is a type of CVD method that can be used to form compound semiconductor films such as Ga2O3 and GaN. In this method, the Ga raw material is reacted with a halide to generate gallium halide gas, which is then supplied onto the substrate for film formation. At the same time, O2 gas is supplied onto the substrate for film formation, and the gallium halide gas reacts with the O2 gas to grow Ga2O3 on the substrate for film formation. This method allows for high speed and thick film growth, and has a wide track record in industrial applications.
[0034] 3 shows an example of a vapor phase growth apparatus (HVPE apparatus) using the HVPE method. The HVPE apparatus 20 includes a reactor 22, a susceptor 26 on which a base substrate 24 for film formation is placed, an oxygen source supply source 30, a carrier gas supply source 28, a GeCl4 supply source 32, a Ga source supply source 34, a heater 36, and a gas exhaust unit 38. The reactor 22 may be any reactor that does not react with the source material, such as a quartz tube. The heater 36 may be any heater that can heat up to at least 700°C (preferably 900°C or higher), such as a resistance heating heater.
[0035] Metal Ga is placed inside the Ga source 34, and a halogen gas or hydrogen halide gas, for example, HCl, is supplied to the Ga source 34. The halogen gas or halogen gas is preferably Cl2 or HCl. The supplied halogen gas or halogen gas reacts with the metal Ga to generate a gallium halide gas, which is supplied to the base substrate 24 for deposition. The gallium halide gas preferably contains GaCl and / or GaCl3. The oxygen source 30 can supply an oxygen source selected from the group consisting of O2, H2O, and N2O, with O2 being preferred. These oxygen source gases are supplied to the base substrate simultaneously with the gallium halide gas. The GeCl4 source 32 supplies GeCl4 vapor generated by bubbling GeCl4 liquid into the reactor 22. The Ga source and oxygen source gas may be supplied together with a carrier gas such as N2 or a rare gas.
[0036] The gas exhaust unit 38 may be connected to a vacuum pump such as a diffusion pump or a rotary pump, and may not only exhaust unreacted gases in the reactor 22 but also control the inside of the reactor 22 to a reduced pressure. This can suppress gas phase reactions and improve the growth rate distribution.
[0037] The base substrate 24 for film formation is heated to a predetermined temperature using the heater 36, and gallium halide gas and oxygen source gas are simultaneously supplied, thereby forming ε-Ga2O3 on the base substrate 24 for film formation. The film formation temperature is not particularly limited as long as ε-Ga2O3 is formed and voids are generated in the film, but is typically 250°C to 900°C. The partial pressures of the Ga source gas and the oxygen source gas are also not particularly limited. For example, the partial pressure of the Ga source gas (gallium halide gas) may be in the range of 0.05 kPa to 10 kPa, and the partial pressure of the oxygen source gas may be in the range of 0.25 kPa to 50 kPa.
[0038] When forming an ε-Ga2O3-based semiconductor film containing a group 14 element as a dopant, or when forming a mixed crystal film with ε-Ga2O3 containing oxides of In or Al, a separate supply source (for example, GeCl4 supply source 32 in FIG. 3) may be provided to supply the halides, or a mixture of halides may be supplied from a Ga raw material supply source 34. In addition, a material containing a group 14 element, In, Al, or the like may be placed in the same place as the metal Ga, reacted with a halogen gas or hydrogen halide gas, and supplied as a halide. The halide gas supplied to the base substrate 24 reacts with the oxygen raw material gas to become an oxide, similar to gallium halide, and is incorporated into the ε-Ga2O3-based semiconductor film.
[0039] The mist CVD method is a method in which a raw material solution is atomized or turned into droplets to generate mist or droplets, and the mist or droplets are transported to a film-forming chamber equipped with a substrate using a carrier gas, and the mist or droplets are thermally decomposed and chemically reacted in the film-forming chamber to form and grow a film on the substrate. This method does not require a vacuum process and can produce a large amount of samples in a short time. FIG. 4 shows an example of a mist CVD apparatus. The mist CVD apparatus 40 shown in FIG. 4 has a mist generating chamber 42 that generates mist M from a carrier gas G and a raw material solution L, and a film-forming chamber 50 that sprays the mist M onto a substrate 56 to form a semiconductor film 58 through thermal decomposition and chemical reaction. The mist generating chamber 42 has a carrier gas inlet 44 through which the carrier gas G is introduced, an ultrasonic vibrator 46 provided in the mist generating chamber 42, and a duct 48 that transports the mist M generated in the mist generating chamber 42 to the film-forming chamber 50. The raw material solution L is accommodated in the mist generating chamber 42. The ultrasonic vibrator 46 is configured to apply ultrasonic vibrations to the raw material solution L to generate mist M together with carrier gas G. The film formation chamber 50 includes a nozzle 52 for spraying the mist M introduced through the duct 48 onto a substrate 56, a stage 54 to which the substrate 56 is fixed, a heater 62 provided near the rear surface of the stage 54 for heating the stage 54 and the substrate 56, and an exhaust port 64 for discharging the carrier gas G.
[0040] The raw material solution L used in the mist CVD method is not limited as long as it is a solution that can obtain an ε-Ga2O3-based semiconductor film, but examples thereof include organometallic complexes and halides of Ga and / or metals that form solid solutions with Ga dissolved in a solvent. An example of an organometallic complex is an acetylacetonate complex. In addition, when a dopant is added to the semiconductor layer, a solution of the dopant component may be added to the raw material solution. Furthermore, an additive such as hydrochloric acid may be added to the raw material solution. Water, alcohol, etc. can be used as the solvent.
[0041] Next, the obtained raw material solution L is atomized or turned into droplets to generate a mist M or droplets. A preferred example of a method for atomizing or turning into droplets is a method of vibrating the raw material solution L using an ultrasonic vibrator 46. The obtained mist M or droplets are then transported to the film formation chamber 50 using a carrier gas G. The carrier gas G is not particularly limited, but one or more of inert gases such as oxygen, ozone, and nitrogen, and reducing gases such as hydrogen can be used.
[0042] The film formation chamber 50 is equipped with a substrate 56. The mist M or droplets transported to the film formation chamber 50 are thermally decomposed and chemically reacted therein to form a semiconductor film 58 on the substrate 56. The reaction temperature varies depending on the type of the raw material solution L, but is preferably 300 to 800°C, and more preferably 400 to 700°C. The atmosphere in the film formation chamber 50 is not particularly limited as long as a desired semiconductor film can be obtained, and is typically selected from an oxygen gas atmosphere, an inert gas atmosphere, a vacuum atmosphere, a reducing atmosphere, and an air atmosphere.
[0043] The semiconductor film thus obtained can be used as it is or divided into a semiconductor element. Alternatively, the semiconductor film may be peeled off from the base substrate to form a single film. In this case, a release layer may be provided in advance on the surface (film formation surface) of the base substrate to facilitate peeling from the base substrate. Examples of such a release layer include a C-injected layer or an H-injected layer provided on the surface of the base substrate. Also, C or H may be injected into the film at the initial stage of film formation, and a release layer may be provided on the semiconductor film side. Furthermore, it is also possible to bond and adhere a support substrate (mounting substrate) different from the base substrate to the surface (i.e., the surface opposite to the base substrate) of the semiconductor film formed on the base substrate, and then peel and remove the base substrate from the semiconductor film. As such a support substrate (mounting substrate), a substrate having a thermal expansion coefficient of 6 to 13 ppm / K at 25 to 400°C, for example, a substrate made of a Cu-Mo composite metal, can be used. Examples of a method for bonding and joining the semiconductor film to the support substrate (mounting substrate) include known methods such as brazing, soldering, and solid-state bonding. Furthermore, an electrode such as an ohmic electrode or a Schottky electrode, or another layer such as an adhesive layer may be provided between the semiconductor film and the supporting substrate.
[0044] In the manufacture of semiconductor elements such as power devices, a functional layer such as a drift layer is formed on a semiconductor film. A known method can be used to form the functional layer such as the drift layer, and preferred examples include the mist CVD method, the HVPE method, the MBE method, the MOCVD method, and the hydrothermal synthesis method, with the mist CVD method or the HVPE method being particularly preferred.
[0045] Composite Board The semiconductor film of the present invention can be manufactured by forming a film of an ε-Ga2O3-based material on a GaN single crystal substrate, preferably as a base substrate. That is, the present invention provides a composite substrate having a two-layer structure composed of a GaN single crystal substrate and the above-mentioned semiconductor film formed on the GaN single crystal substrate.
[0046] The GaN single crystal substrate is preferably circular. The off-angle distribution on the surface of the GaN single crystal substrate is preferably 0.2° or less, more preferably 0.1° or less. Since the off-angle distribution is better to be small, the lower limit is not particularly limited, and is ideally 0°, but typically 0.01° or more. The off-angle distribution and off-angle of the GaN single crystal substrate can be obtained in the same manner as the off-angle distribution and off-angle of the semiconductor film described above. That is, the off-angle distribution is calculated by dividing the maximum off-angle θ at the center point X and the four peripheral points A, B, C, and D of the surface of the GaN single crystal substrate by the maximum off-angle θ at the center point X and the four peripheral points A, B, C, and D of the surface of the GaN single crystal substrate. max and the minimum value θ min The off-angle of the GaN single crystal substrate is defined as the inclination angle of the crystal axis oriented in the approximately normal direction of the GaN single crystal substrate with respect to the normal line of the substrate surface of the GaN single crystal substrate. The outer periphery points A, B, C, and D are determined such that i) a straight line connecting the outer periphery points A and C and a straight line connecting the outer periphery points B and D intersect at a right angle at the center point X, and ii) the shortest distance from the outer edge of the semiconductor film to the outer periphery points A, B, C, and D is 1 / 5 of the radius of the semiconductor film. On the surface of the GaN single crystal substrate, the arithmetic mean angle of the off-angles at the center point X and the outer periphery points A, B, C, and D is preferably 0.01 to 0.5°, more preferably 0.02 to 0.45°. The "circular shape" of the GaN single crystal substrate does not need to be a perfect circular shape, as with the "circular shape" of the semiconductor film described above, and may be an approximately circular shape that can be recognized as being approximately circular overall. EXAMPLES
[0047] The present invention will now be further illustrated by the following examples.
[0048] Example 1 (1) Preparation of ε-Ga2O3-based semiconductor films by mist CVD method (1a) Preparation of the base substrate As the base substrate, a commercially available GaN single crystal substrate was prepared, having a thickness of 0.35 mm and a diameter of 5.08 cm, and having the off-angle and off-angle distribution shown in Table 1. The method for measuring the off-angle and off-angle distribution of the GaN single crystal substrate will be described later.
[0049] (1b) Preparation of raw solution Metal Ga was added to hydrochloric acid and stirred at room temperature for three weeks to obtain a gallium chloride solution with a gallium ion concentration of 3 mol / L. Water was added to the obtained gallium chloride solution to adjust the aqueous solution to a gallium ion concentration of 50 mmol / L. Tin (II) chloride was added to this aqueous solution to a concentration of 1.0 mmol / L, and then ammonium hydroxide was added to adjust the pH to 4.0 to obtain the raw solution.
[0050] (1c) Preparation for film formation A mist CVD apparatus 40 having a configuration shown in FIG. 4 was prepared. The configuration of the mist CVD apparatus 40 was as described above. In the mist CVD apparatus 40, the raw material solution L obtained in (1b) above was accommodated in the mist generating chamber 42. A c-plane GaN single crystal substrate having a diameter of 50.8 mm (2 inches) was set on the stage 54 as the substrate 56, and the distance between the tip of the nozzle 52 and the substrate 56 was set to 110 mm. The temperature of the stage 54 was raised to a predetermined temperature (film formation temperature shown in Table 1) by the heater 62, and the temperature was maintained for 30 minutes to stabilize. The flow rate control valve (not shown) was opened to supply nitrogen gas as the carrier gas G into the film formation chamber 50 via the mist generating chamber 42, and the atmosphere in the film formation chamber 50 was sufficiently replaced with the carrier gas G. Thereafter, the flow rate of the carrier gas G was adjusted to 2.0 L / min.
[0051] (1d) Film formation The raw material solution L was atomized by the ultrasonic vibrator 46, and the generated mist M was introduced into the film formation chamber 50 by the carrier gas G. The mist M was reacted in the film formation chamber 50, particularly on the surface of the substrate 56, to form a semiconductor film 58 on the substrate 56. The film formation time was as shown in Table 1. In this way, a composite substrate 60 consisting of the substrate 56 and the semiconductor film 58 formed thereon was obtained.
[0052] (2) Evaluation (2a) Surface EDX As a result of performing a composition analysis by energy dispersive X-ray analysis (EDX) on the surface of the obtained semiconductor film, only Ga and O were detected. From this, it was found that the obtained semiconductor film is composed of Ga oxide.
[0053] (2b) Surface EBSD Using a scanning electron microscope (SEM) (SU-5000, manufactured by Hitachi High-Technologies Corporation) equipped with an electron backscatter diffraction device (EBSD) (Nordlys Nano, manufactured by Oxford Instruments), inverse pole figure orientation mapping of the surface of the Ga oxide film was performed in a field of view of approximately 25 μm × 20 μm. Using the software (Twist) attached to the apparatus, the crystal information of the space group, unit cell parameters (sides and angles), and atomic positions of ε-Ga2O3 (hexagonal crystal) described in Non-Patent Document 2 (F. Mezzadri, et al., "Crystal Structure and Ferroelectric Properties of ε-Ga2O3Films Grown on (0001)-Sapphire," Inorg. Chem. 2016, 55, 12079-12084) was registered in the database, and EBSD measurement was performed using this.
[0054] The conditions for this EBSD measurement were as follows. <EBSD measurement conditions> ·Acceleration voltage: 15 kV ·Spot intensity: 70 ·Working distance: 22.5 mm ·Step size: 0.5 μm ·Sample tilt angle: 70° ·Measurement program: Aztec (version 3.3)
[0055] From the obtained inverse pole figure orientation mapping, it was found that the Ga oxide film has a biaxially oriented crystal structure with the c-axis oriented in the substrate normal direction and also oriented in the plane. From these results, it was confirmed that the obtained semiconductor film is an oriented film with a crystal structure composed of ε-Ga2O3.
[0056] (2c) Measurement of off-angle and off-angle distribution At the center point X and peripheral points A, B, C, and D of the surface of the GaN single crystal substrate or semiconductor film, the angular difference between the c-axis direction of the GaN single crystal substrate or the c-axis direction of the ε-Ga2O3 semiconductor film and the direction perpendicular to the GaN single crystal substrate surface, i.e., the off-angle, was measured. The off-angle distribution was also measured. The off-angle measurement was performed on the GaN (002) plane or the ε-Ga2O3 (004) plane using an automatic X-ray crystal orientation measurement device (FSAS III, manufactured by Rigaku) with a sampling width of 0.01° and a scan speed of 10° / min. The off-angles obtained at the center point X and peripheral points A, B, C, and D were defined as θ X , θ A , θ B , θ C , and θ D The arithmetic mean of these off angles is the "off angle (°)" of the GaN single crystal substrate or the ε-Ga2O3 semiconductor film, and the maximum value of these off angles is θ max and the minimum value θ min The difference between the above values was defined as the "off-angle distribution (°)" of the GaN single crystal substrate or the ε-Ga2O3 semiconductor film. Note that the off-angle in this specification only measures the difference in angle between the direction perpendicular to the GaN single crystal substrate surface and the c-axis direction of the GaN single crystal substrate or the c-axis direction of the ε-Ga2O3 semiconductor film, and does not measure the tilt direction of the off-angle. The results are shown in Tables 1 and 2.
[0057] (2d) Number of cracks in ε-Ga2O3 semiconductor film The number of cracks in the ε-Ga2O3 semiconductor film was determined using an industrial microscope (Nikon ECLIPSE LV150N). The entire film surface was observed in polarized and differential interference mode with a 10x eyepiece and a 5x objective lens, and if a crack was observed, the objective lens was changed to 10x and an image was taken. At this time, only cracks with a length of 50 μm or more were counted as cracks. In addition, if the shortest distance from one crack to another was 500 μm or less, it was considered to be one crack. The final crack count was calculated by counting the number of cracks when observing the entire film surface excluding the area within 2 mm from the outer periphery of the semiconductor film (i.e., the outer periphery of the substrate), regardless of the size of the semiconductor film, and was calculated based on the number of cracks observed per unit area of 20 cm of the semiconductor film. 2The number of cracks was calculated by converting it into the number of cracks per unit. The results are shown in Table 2. The obtained semiconductor film had a reduced number of cracks.
[0058] (2e) Arithmetic mean roughness Ra of ε-Ga2O3 semiconductor film The surface roughness of the ε-Ga2O3 semiconductor film was measured. Specifically, the surface roughness Ra of the film surface in an area of 140 μm × 100 μm was measured using a surface roughness measuring instrument (Zygo, NewView7300) in accordance with JIS B 0601 (2001). The results are shown in Table 2.
[0059] (2f) Thickness of ε-Ga2O3 semiconductor film After embedding the composite substrate obtained in (1c) above in resin, a cross section was prepared using a microcutter, and a cross section polisher (IB-19500CP, manufactured by JEOL) was used to prepare a specimen for cross section observation. A backscattered electron image of the obtained cross section was taken using a scanning electron microscope (SEM) (SU-5000, manufactured by Hitachi High-Technologies). At this time, the GaN single crystal and the ε-Ga2O3 semiconductor film in the composite substrate can be easily distinguished from each other due to the contrast difference. The thickness of the ε-Ga2O3 semiconductor film was measured from this cross-sectional SEM image. The results are shown in Table 2.
[0060] Example 2 Instead of the base substrate in (1a) above, a commercially available GaN single crystal substrate (with a smaller off angle and slightly larger off angle distribution than in Example 1) having the off angle and off angle distribution shown in Table 1 was used, and the deposition time in (1d) above was changed to 60 minutes as shown in Table 1 (deposition time was extended), but the same procedures were followed as in Example 1 to prepare a semiconductor film and a composite substrate, and various evaluations were performed. The obtained semiconductor film was confirmed to be an oriented film with a crystal structure composed of ε-Ga2O3. In addition, the number of cracks in this semiconductor film was reduced (although more than in Example 1). The results are shown in Tables 1 and 2.
[0061] Example 3 Except for changing the film formation temperature in (1c) above to 520°C (raising the film formation temperature) as shown in Table 1, the semiconductor film and composite substrate were prepared and various evaluations were performed in the same manner as in Example 1. The obtained semiconductor film was confirmed to be an oriented film with a crystal structure composed of ε-Ga2O3. In addition, this semiconductor film had a smaller arithmetic mean roughness Ra and fewer cracks than Example 1. The results are shown in Tables 1 and 2.
[0062] Example 4 The semiconductor film and composite substrate were prepared and various evaluations were performed in the same manner as in Example 1, except that a GaN single crystal substrate (with a smaller off angle than in Example 1) having the off angle and off angle distribution shown in Table 1 was used instead of the base substrate in (1a) above. The obtained semiconductor film was confirmed to be an oriented film with a crystal structure composed of ε-Ga2O3. In addition, this semiconductor film had fewer cracks than Example 1. The results are shown in Tables 1 and 2.
[0063] Example 5 Except for changing the deposition time in (1d) above to 120 minutes as shown in Table 1 (lengthening the deposition time), the semiconductor film and composite substrate were prepared and various evaluations were performed in the same manner as in Example 1. The obtained semiconductor film was confirmed to be an oriented film with a crystal structure composed of ε-Ga2O3. In addition, this semiconductor film was thicker than in Example 1, and the number of cracks was fewer (although more than in Example 1). The results are shown in Tables 1 and 2.
[0064] Example 6 Except for changing the deposition time in (1d) above to 30 minutes as shown in Table 1 (shortening the deposition time), the semiconductor film and composite substrate were prepared and various evaluations were performed in the same manner as in Example 1. The obtained semiconductor film was confirmed to be an oriented film with a crystal structure composed of ε-Ga2O3. In addition, this semiconductor film had a smaller arithmetic mean roughness Ra than Example 1, was also reduced in thickness, and was almost free of cracks. The results are shown in Tables 1 and 2.
[0065] Example 7 (comparison) The semiconductor film and composite substrate were prepared and evaluated in the same manner as in Example 1, except that a commercially available GaN single crystal substrate (with a smaller off angle and a larger off angle distribution than in Example 1) having the off angle and off angle distribution shown in Table 1 was used instead of the base substrate in (1a) above. The obtained semiconductor film was confirmed to be an oriented film with a crystal structure composed of ε-Ga2O3. In addition, this semiconductor film had a significantly larger number of cracks than Examples 1 to 6. The results are shown in Tables 1 and 2.
[0066] [Table 1]
[0067] [Table 2]
Claims
1. ε-Ga 2 O 3 , or ε-Ga 2 O 3 A circular semiconductor film having a main phase of a crystal composed of a system solid solution, The off-angle distribution on the surface of the semiconductor film is 0.25° or less, and the off-angle distribution is a maximum value θ of the off-angle at a center point X and four outer periphery points A, B, C, and D on the surface of the semiconductor film. max and the minimum value θ min the off angle is defined as an inclination angle of a crystal axis oriented in a direction approximately normal to the semiconductor film with respect to a normal to the film surface of the semiconductor film, and the outer periphery points A, B, C, and D are determined such that i) a straight line connecting the outer periphery points A and C and a straight line connecting the outer periphery points B and D intersect at a right angle at the center point X, and ii) the shortest distance from the outer edge of the semiconductor film to each of the outer periphery points A, B, C, and D is 1 / 5 of the radius of the semiconductor film, When observing the entire surface of the semiconductor film excluding a region within 2 mm from the outer periphery, 2 1. A semiconductor film having 20 or less cracks each having a length of 50 μm or more, provided that a crack is considered to be one crack if the shortest distance from one crack to another is 500 μm or less.
2. 2. The semiconductor film according to claim 1, wherein the arithmetic mean roughness Ra of the surface of the semiconductor film is 0.1 to 50 nm.
3. 3. The semiconductor film according to claim 1, wherein an arithmetic mean angle of the off angles at the center point X and the outer periphery points A, B, C and D is 0.01 to 0.5°.
4. The semiconductor film according to claim 1 , wherein the off-angle distribution is 0.15° or less.
5. The semiconductor film according to claim 1 , wherein the thickness of the semiconductor film is 200 nm or more.
6. 3. A composite substrate having a two-layer structure comprising a GaN single crystal substrate and the semiconductor film according to claim 1 or 2 formed on the GaN single crystal substrate.
Citation Information
Patent Citations
Gallium oxide semiconductor and preparation method thereof
CN110085658A
Gallium oxide semiconductor lamination structure and preparation method thereof
CN110085661A
Application of gallium oxide to piezoelectric material, piezoelectric film and piezoelectric device
CN111640857A
Method for regulating and controlling photoelectric response performance of epsilon-phase gallium oxide through oxygen vacancy concentration
CN113066902A
Motor-operated remote-controlled mirror device
JP1989036538A