Method for tensioning single crystal silicon rod and single crystal silicon rod

By controlling oxygen concentration through magnetic field adjustments during single crystal silicon rod growth, the method addresses the non-uniform BMD density issue, improving semiconductor device quality and productivity.

JP7591166B2Active Publication Date: 2024-11-27XIAN ESWIN MATERIAL TECHNOLOGY CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023569755
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-11-25
Filing Date
2022-10-28
Publication Date
2024-11-27
Estimated Expiration
2042-10-28

AI Technical Summary

Technical Problem

The challenge in semiconductor manufacturing is achieving uniform bulk micro defect (BMD) density distribution in epitaxial silicon wafers, which is compromised by high-temperature processes that reduce BMD cores, leading to inadequate gettering of heavy metal impurities and reduced quality of semiconductor devices.

Method used

A method for stretching single crystal silicon rods by adjusting the horizontal magnetic field position and strength during growth to control oxygen concentration, thereby suppressing nitrogen segregation and achieving uniform BMD density distribution.

Benefits of technology

The method ensures a uniform BMD density distribution along the axial direction of the silicon rod, enhancing the gettering capability and improving the quality and productivity of semiconductor devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007591166000001
    Figure 0007591166000001
  • Figure 0007591166000002
    Figure 0007591166000002
  • Figure 0007591166000003
    Figure 0007591166000003
Patent Text Reader

Abstract

The embodiments of the present disclosure disclose a method for pulling a single crystal silicon rod and a single crystal silicon rod, which includes: setting a horizontal magnetic field such that a starting height of the horizontal magnetic field is higher than a free surface of a silicon melt in an initial stage of isodiametric growth of the single crystal silicon rod; and changing a control strength of the horizontal magnetic field on the convection of the silicon melt so that the oxygen concentration in the axial direction from the head to the tail of the single crystal silicon rod tends to decrease in the isodiametric growth process of the single crystal silicon rod.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] (CROSS REFERENCE TO RELATED APPLICATIONS) This disclosure claims priority to a Chinese patent application filed in China on November 25, 2021, with application number 202111411291.X, the entire contents of which are incorporated herein by reference.

[0002] TECHNICAL FIELD The embodiments of the present disclosure relate to the field of semiconductor manufacturing technology, and more particularly to a method for drawing a single crystal silicon rod and a single crystal silicon rod. [Background technology]

[0003] In recent years, with the progress of miniaturization in the manufacturing process of semiconductor devices, the demands on the necessary silicon wafers are increasing. Not only are there demands for the surface region of the silicon wafer to have few defects, or even to be free of defects, but the silicon wafer is also required to have sufficient bulk micro defects (BMD) to protect the silicon wafer region where electronic components are arranged from contamination by heavy metal impurities.

[0004] Epitaxial silicon wafers are formed by growing a single crystal layer (also called an epitaxial layer) on a silicon wafer by a deposition reaction, and because the epitaxial layer has high crystal perfection and almost no defects, epitaxial silicon wafers are currently widely used as substrate materials for semiconductor devices. However, heavy metal impurities contained in silicon wafers are an important factor that affects the quality of semiconductor devices, so the content of heavy metal impurities needs to be reduced as much as possible during the manufacturing process of silicon wafers. Currently, it is known that if a sufficient amount of BMDs are formed inside a silicon wafer, these BMDs have an intrinsic gettering (IG) effect of capturing heavy metal impurities, and the problem of defective quality of semiconductor devices due to heavy metal impurities can be significantly improved. However, during the epitaxial growth process, the silicon wafer is exposed to a high-temperature environment of 1000° C. or more, and small BMD cores are removed at this high temperature, so that a sufficient amount of BMD cores cannot be provided in the epitaxial silicon wafer. In this case, a sufficient density of BMDs cannot be generated when manufacturing a semiconductor device using the epitaxial silicon wafer, and the quality of the manufactured semiconductor device is further reduced.

[0005] In order to solve the problem of the decrease in BMD density in epitaxial silicon wafers, nitrogen doping is generally performed during the drawing process of single crystal silicon rods to obtain stable BMD cores, but currently, the density of BMDs in nitrogen-doped single crystal silicon rods increases with increasing nitrogen concentration. Due to the process requirements of clients for semiconductor devices, the requirements for the uniformity of BMD density are also becoming increasingly strict, in which case the single crystal silicon rods cannot meet the process requirements of certain clients without loss, resulting in low productivity and high shipping costs. Summary of the Invention [Problem to be solved by the invention]

[0006] In view of this, it is desirable for the embodiments of the present disclosure to provide a method for tensioning a single crystal silicon rod and a single crystal silicon rod that can exhibit a tendency to gradually decrease the oxygen concentration in the axial direction from the head to the tail of the single crystal silicon rod, so that the BMD density distribution in the axial direction of the single crystal silicon rod becomes more uniform. [Means for solving the problem]

[0007] The technical solutions according to the embodiments of the present disclosure are realized as follows:

[0008] In a first aspect, embodiments of the present disclosure provide a method of tensioning a single crystal silicon rod, the method comprising: In the initial stage of the uniform diameter growth of the single crystal silicon rod, the starting height of the horizontal magnetic field is set higher than the free surface of the silicon melt; During the isodiametric growth process of the single crystal silicon rod, changing the height or strength of the horizontal magnetic field to change the control intensity on the convection of the silicon molten liquid so that the oxygen concentration in the axial direction tends to decrease from the head to the tail of the single crystal silicon rod.

[0009] In a second aspect, embodiments of the present disclosure provide a single crystal silicon rod produced by the tensioning method according to the first aspect. Effect of the Invention

[0010] In the embodiments of the present disclosure, a tensile method for a single crystal silicon rod and a single crystal silicon rod are provided, in which, in the initial stage of isodiametric growth of the single crystal silicon rod, a horizontal magnetic field is set at a position higher than the free surface of the silicon melt, and the height or strength of the horizontal magnetic field is changed during the isodiametric growth process so that the oxygen concentration in the axial direction gradually decreases from the head to the tail of the single crystal silicon rod, thereby suppressing an increase in BMD density due to nitrogen concentration segregation, and ultimately making the BMD density distribution in the axial direction of the entire single crystal silicon rod more uniform. [Brief description of the drawings]

[0011] [Figure 1] FIG. 1 is a structural schematic diagram of a crystal tension furnace apparatus according to an embodiment of the present disclosure. [Diagram 2] FIG. 1 is a schematic diagram of the change trend of nitrogen concentration according to the length of a single crystal silicon rod according to an embodiment of the present disclosure. [Diagram 3] FIG. 2 is a schematic diagram of the change trend of oxygen concentration in the axial direction from the head to the tail of a related single crystal silicon rod according to an embodiment of the present disclosure. [Figure 4] FIG. 1 is a flow diagram of a method for tensioning a single crystal silicon rod according to an embodiment of the present disclosure. [Diagram 5] FIG. 2 is a schematic diagram of the height of a horizontal magnetic field at an initial stage of isodiametric growth of a single crystal silicon rod according to an embodiment of the present disclosure. [Figure 6] FIG. 13 is a schematic diagram showing a change trend of oxygen concentration in the axial direction from the head to the tail of a produced single crystal silicon rod in the case where the magnetic field strength of the horizontal magnetic field is kept constant and the height of the horizontal magnetic field is gradually decreased during the isodiametric growth process of the single crystal silicon rod according to the embodiment of the present disclosure. [Figure 7] FIG. 10 is a schematic diagram showing a change trend of oxygen concentration in the axial direction from the head to the tail of a produced single crystal silicon rod in a process of isodiametric growth of a single crystal silicon rod according to an embodiment of the present disclosure, in which the height of the horizontal magnetic field is kept constant and the magnetic field strength of the horizontal magnetic field is gradually increased. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The technical solutions in the embodiments of the present disclosure will be described clearly and completely below with reference to the drawings in the embodiments of the present disclosure.

[0013] FIG. 1 shows a crystal tension furnace apparatus 1 according to an embodiment of the present disclosure. As shown in FIG. 1, the crystal tension furnace apparatus 1 mainly includes a quartz crucible 10 and a graphite crucible 20. Here, the graphite crucible 20 is used to support and fix the quartz crucible 10. It can be understood that the crystal tension furnace apparatus 1 shown in FIG. 1 may also include other structures not shown in FIG. 1, such as a crucible lifting device. The embodiment of the present disclosure will not be specifically described therefor.

[0014] When the nitrogen-doped single crystal silicon rod S is stretched using the above-mentioned crystal stretching furnace apparatus 1, the nitrogen concentration of the single crystal silicon rod S reaches a predetermined target concentration at the initial crystal growth stage during crystal growth, but as the crystal growth process progresses, the nitrogen concentration in the single crystal silicon rod gradually increases as the length (ingot length) of the single crystal silicon rod S increases due to nitrogen segregation, as shown in Fig. 2. Therefore, the BMD density in the single crystal silicon rod S obtained by stretching tends to gradually increase in the axial direction from the head to the tail. According to the related art, the higher the oxygen concentration in the single crystal silicon rod S, the higher the BMD density contained therein. Therefore, by controlling the change tendency of the oxygen concentration in the single crystal silicon rod S, the increase tendency of the BMD density in the axial direction of the single crystal silicon rod S can be suppressed.

[0015] Currently, in the pulling method of the single crystal silicon rod S based on the direct drawing (Czochralski, CZ) method, the change tendency of the oxygen concentration in the single crystal silicon rod S is generally adjusted by using a process method such as rotating the quartz crucible or adjusting the argon gas flow rate. However, with these process methods, it is difficult for the oxygen concentration to exhibit a change tendency opposite to that of the nitrogen concentration. In general, the oxygen concentration in the axial direction from the head to the tail of the single crystal silicon rod S tends to fluctuate up and down within a certain range, specifically as shown in FIG. 3, and there is a limit to the reduction in the oxygen concentration.

[0016] Based on the above description, a method for tensioning a single crystal silicon rod according to an embodiment of the present disclosure is shown in Figure 4. The method includes the following steps S401 to S402.

[0017] In S401, in the initial stage of isodiametric growth of a single crystal silicon rod, the starting height of the horizontal magnetic field is set to be higher than the free surface of the silicon melt.

[0018] In S402, the control strength of the horizontal magnetic field on the convection of the silicon melt is changed so that the oxygen concentration in the axial direction from the head to the tail of the single crystal silicon rod tends to decrease during the isodiametric growth process of the single crystal silicon rod.

[0019] In the technical solution shown in FIG. 4, in the initial stage of isodiametric growth of the single crystal silicon rod S, the horizontal magnetic field is set at a position higher than the free surface of the silicon melt MS, and the control strength of the horizontal magnetic field on the convection of the silicon melt MS is changed during the isodiametric growth process, thereby weakening the convection degree of the silicon melt and causing a decrease in the oxygen concentration at the free surface of the silicon melt MS. The oxygen concentration in the axial direction is gradually decreased from the head to the tail of the single crystal silicon rod S, thereby suppressing the increase in BMD density due to nitrogen concentration segregation, and finally making the BMD density distribution in the axial direction of the entire single crystal silicon rod S more uniform.

[0020] In the embodiments of the present disclosure, the head of the single crystal silicon rod S refers to the portion of the single crystal silicon rod obtained by pulling at the initial stage of isodiametric growth, and the tail of the single crystal silicon rod S refers to the portion of the single crystal silicon rod obtained by pulling at the final stage of isodiametric growth.

[0021] To implement the embodiment of the present disclosure, as specifically shown in Fig. 5, a pair of excitation coils 30 can be installed around the circumference of the graphite crucible 20 to apply a horizontal magnetic field to the silicon melt MS in the quartz crucible 10, where the dotted line in the figure represents the horizontal plane 40 of the horizontal magnetic field. In the embodiment of the present disclosure, the distance H between the horizontal plane 40 and the free surface of the silicon melt MS is used to characterize the position of the horizontal magnetic field (Maximum Gauss Position, MGP), and as can be understood, the horizontal magnetic field is a three-dimensional structure that occupies a certain space, and the MGP refers to the middle position of the entire horizontal magnetic field.

[0022] In the embodiment of the present disclosure, it is defined that when the horizontal plane 40 of the horizontal magnetic field overlaps with the free surface of the silicon melt MS, the height of the horizontal magnetic field is 0, and when the horizontal plane 40 of the horizontal magnetic field is higher than the free surface of the silicon melt MS, the height of the horizontal magnetic field is greater than 0. For example, when the horizontal plane 40 of the horizontal magnetic field is 100 mm higher than the free surface of the silicon melt MS, the height of the horizontal magnetic field is +100 mm. Similarly, when the horizontal plane 40 of the horizontal magnetic field is lower than the free surface of the silicon melt MS, the height of the horizontal magnetic field is less than 0. For example, when the horizontal plane 40 of the horizontal magnetic field is 100 mm lower than the free surface of the silicon melt MS, the height of the horizontal magnetic field is -100 mm.

[0023] In the embodiment of the present disclosure, the control strength of the silicon melt MS convection by the horizontal magnetic field means a characterization quantity of the degree of control of the silicon melt MS convection by the horizontal magnetic field. When the control strength of the silicon melt MS convection by the horizontal magnetic field increases, the degree of convection of the silicon melt MS weakens, leading to a decrease in the oxygen concentration at the free surface of the silicon melt MS, and further, the oxygen concentration content in the axial direction of the single crystal silicon rod S gradually decreases from the head to the tail. For example, in the embodiment of the present disclosure, as shown in FIG. 5, in the initial stage of isodiametric growth of the single crystal silicon rod S, when the horizontal plane 40 of the horizontal magnetic field is higher than the free surface of the silicon melt MS, the quartz crucible 10 continues to be in the upward process during the pulling process of the single crystal silicon rod S so that the free surface of the silicon melt MS is basically kept at the same position. In this case, the control degree of the silicon melt MS convection by the horizontal magnetic field P can be reinforced by decreasing the height of the horizontal magnetic field or increasing the magnetic field strength.

[0024] Optionally, in embodiments of the present disclosure, to reduce the height of the horizontal magnetic field, In some possible implementations, changing the control strength of the horizontal magnetic field on the convection of the silicon melt so that the oxygen concentration in the axial direction from the head to the tail of the single crystal silicon rod tends to decrease during the isodiametric growth of the single crystal silicon rod is: In the process of growing the single crystal silicon rod in an equal diameter, the oxygen concentration in the axial direction of the single crystal silicon rod S from the head to the tail tends to decrease. The magnetic field strength of the horizontal magnetic field is kept constant, and the height of the horizontal magnetic field is gradually decreased to increase the control strength of the horizontal magnetic field on the convection of the silicon melt.

[0025] Specifically, in order to change the height of the horizontal magnetic field, the crystal pulling furnace apparatus 1 is further equipped with a magnetic field moving unit 50 as shown in Fig. 5. The magnetic field moving unit 50 is used to move the excitation coil 30 to change the height of the horizontal magnetic field during the pulling process of the single crystal silicon rod S.

[0026] Specifically, as shown in FIG. 6, when the magnetic field strength of the horizontal magnetic field remains constant, the oxygen concentration in the axial direction from the head to the tail of the single crystal silicon rod S tends to decrease in the process of gradually decreasing the horizontal magnetic field.

[0027] For the above possible implementations, in some examples, the rate of decrease of the horizontal magnetic field is between 0.02 mm / h and 0.12 mm / h.

[0028] Regarding the above possible implementation manner, in some examples, the tensioning method further comprises: This includes making the horizontal plane of the horizontal magnetic field equal to or greater than the free surface of the silicon melt at the end of the isodiametric growth of the single crystal silicon rod. That is, at the end of the isodiametric growth of the single crystal silicon rod S, the horizontal plane 40 of the horizontal magnetic field overlaps at least with the free surface of the silicon melt MS. That is, the height of the horizontal magnetic field is at least 0. Of course, at the end of the isodiametric growth of the single crystal silicon rod S, the height of the horizontal magnetic field may be greater than 0.

[0029] Optionally, in embodiments of the present disclosure, to increase the magnetic field strength of the horizontal magnetic field, In some possible implementations, changing the control strength of the horizontal magnetic field on the convection of the silicon melt so that the oxygen concentration in the axial direction from the head to the tail of the single crystal silicon rod tends to decrease during the isodiametric growth of the single crystal silicon rod is: In the process of growing the single crystal silicon rod in an equal diameter, the oxygen concentration in the axial direction of the single crystal silicon rod tends to decrease from the head to the tail. The height of the horizontal magnetic field is kept constant, and the magnetic field strength of the horizontal magnetic field is gradually increased to increase the strength of control exerted by the horizontal magnetic field on the convection of the silicon melt.

[0030] For example, in embodiments of the present disclosure, the input current of the excitation coil 30 may be increased to increase the magnetic field strength of the horizontal magnetic field.

[0031] Specifically, as shown in FIG. 7, when the height of the horizontal magnetic field remains constant, in the process of gradually increasing the magnetic field strength of the horizontal magnetic field, the oxygen concentration in the axial direction from the head to the tail of the single crystal silicon rod S tends to decrease.

[0032] For the above possible implementations, in some examples, the frequency of increase of the magnetic field strength of the horizontal magnetic field is between 0.2 G / h and 0.6 G / h.

[0033] Regarding the above possible implementation manner, in some examples, the magnetic field strength of the horizontal magnetic field is 4000 Gaussian (G) or less at the end of the isodiametric growth stage of the single crystal silicon rod. That is, in the embodiment of the present disclosure, in order to facilitate the growth of the single crystal silicon rod S, the magnetic field strength of the horizontal magnetic field is set to 4000 G or less at the end of the isodiametric growth stage of the single crystal silicon rod S.

[0034] Optionally, in an embodiment of the present disclosure, for the single crystal silicon rod having a diameter of 300 mm, during the initial stage of isodiametric growth of the single crystal silicon rod, the starting height of the horizontal magnetic field is +100 mm to +200 mm, and the magnetic field strength of the horizontal magnetic field is 3000 G to 4000 G.

[0035] In the embodiment of the present disclosure, when a single crystal silicon rod S having a diameter of 300 mm is pulled, in the initial stage of isodiametric growth, the starting height of the horizontal magnetic field is +100 mm to +200 mm, the magnetic field strength of the horizontal magnetic field is 3000 G to 4000 G, and in the process of isodiametric growth, the magnetic field strength of the horizontal magnetic field is kept constant and the horizontal magnetic field is gradually decreased at a decreasing rate of 0.02 mm / h to 0.12 mm / h, so that the horizontal surface 40 of the horizontal magnetic field gradually approaches the free surface of the silicon melt MS, thereby reinforcing the control strength of the horizontal magnetic field on the convection of the silicon melt MS, weakening the convection degree of the silicon melt MS, and further, the oxygen concentration content in the axial direction from the head to the tail of the single crystal silicon rod S can be gradually decreased. In the final stage of isodiametric growth, the horizontal surface 40 of the horizontal magnetic field overlaps at least with the free surface of the silicon melt MS.

[0036] Meanwhile, in the embodiment of the present disclosure, when pulling a single crystal silicon rod S having a diameter of 300 mm, in the initial stage of isodiametric growth, the starting height of the horizontal magnetic field is +100 mm to +200 mm, and the magnetic field strength of the horizontal magnetic field is 3000 G to 4000 G. During the isodiametric growth process, the height of the horizontal magnetic field is kept constant, and the magnetic field strength of the horizontal magnetic field is gradually increased at an increasing frequency of 0.2 G / h to 0.6 G / h, thereby reinforcing the control strength of the horizontal magnetic field on the convection of the silicon melt MS, weakening the degree of convection of the silicon melt MS, and further allowing the oxygen concentration content in the axial direction to gradually decrease from the head to the tail of the single crystal silicon rod S. At the end stage of the isodiametric growth, the magnetic field strength of the horizontal magnetic field is set to 4000 G or less.

[0037] Finally, an embodiment of the present disclosure further provides a single crystal silicon rod, which is manufactured by the tensioning method described in the above technical solution.

[0038] In addition, the technical solutions described in the embodiments of the present disclosure can be arbitrarily combined if they do not conflict with each other.

[0039] The above are only specific embodiments of the present disclosure, but the scope of protection of the present disclosure is not limited thereto, and within the technical scope disclosed in the present disclosure, those skilled in the art can easily think of modifications and replacements, all of which should be included in the scope of protection of the present disclosure. Therefore, the scope of protection of the present disclosure should be in accordance with the claims.

Claims

1. 1. A method for tensioning a single crystal silicon rod, comprising the steps of: The tension method comprises: In the initial stage of the isodiametric growth of the single crystal silicon rod, the starting height of the horizontal magnetic field is set higher than the free surface of the silicon melt, and the position of the horizontal magnetic field is the central position of the entire horizontal magnetic field; suppressing an increase in BMD density due to nitrogen concentration segregation by changing a control strength of the horizontal magnetic field on the convection of the silicon melt so that the oxygen concentration in the axial direction of the single crystal silicon rod tends to decrease from the head to the tail during the isodiametric growth of the single crystal silicon rod; In the process of growing the single crystal silicon rod in an equal diameter direction, the control strength of the horizontal magnetic field on the convection of the silicon melt is changed so that the oxygen concentration in the axial direction of the single crystal silicon rod tends to decrease from the head to the tail. the height of the horizontal magnetic field is kept constant and the magnetic field strength of the horizontal magnetic field is gradually increased to increase the control strength of the horizontal magnetic field on the convection of the silicon melt, so that, during the isodiametric growth process of the single crystal silicon rod, the oxygen concentration in the axial direction tends to decrease from the head to the tail of the single crystal silicon rod, wherein the frequency of increase in the magnetic field strength of the horizontal magnetic field is from 0.2 G / h to 0.6 G / h.

2. The tensioning method further comprises: and at the end of the uniform diameter growth of the single crystal silicon rod, the height of the horizontal magnetic field is set to be equal to or higher than the free surface of the silicon melt. The tensioning method according to claim 1.

3. The tensioning method further comprises: and at the end of the equal diameter growth of the single crystal silicon rod, the magnetic field strength of the horizontal magnetic field is set to 4000 G or less. The tensioning method according to claim 1.

4. For the single crystal silicon rod having a diameter of 300 mm, in the initial stage of isodiametric growth of the single crystal silicon rod, the starting height of the horizontal magnetic field is set to +100 mm to +200 mm, and the magnetic field strength of the horizontal magnetic field is set to 3000 G to 4000 G. The tensioning method according to claim 1.

Citation Information

Patent Citations

  • Single crystal pulling apparatus

    JP1985027682A

  • Pulling-up method of semiconductor single crystal

    JP1992055388A

  • Silicon single crystal and its growing method

    JP2010024120A

  • Growing apparatus and single-crystal ingot growing method using the same

    US20190017191A1

  • US2021/79553A1