Method for producing high purity aluminum material - Patent Application 20070123633
The method addresses the high costs and complexity of existing alumina production by using selective extractions and purifications to achieve 99.99% purity alumina and aluminum salts efficiently.
Patent Information
- Application Number
- JP2023575514
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-07-05
- Filing Date
- 2022-07-05
- Publication Date
- 2024-11-27
- Estimated Expiration
- 2042-07-05
AI Technical Summary
Existing methods for producing high purity alumina and aluminum salts are costly due to complex unit operations, significant capital and operating expenses, and the need to recycle hydrogen chloride gas, while achieving the required purity levels of 99.99% remains challenging.
A method involving liquid-liquid and liquid-solid extractions using selective extractants, followed by scrubbing and stripping processes to reduce metal impurities, and subsequent precipitation and calcination to produce high purity alumina and aluminum salts.
The method effectively reduces metal impurities, achieving high purity levels of 99.99% alumina and aluminum salts with reduced operational costs by simplifying the process and eliminating the need for hydrogen chloride gas recycling.
Smart Images

Figure 0007591172000008 
Figure 0007591172000009 
Figure 0007591172000010
Abstract
Description
[Technical field]
[0001] The present disclosure relates to methods for producing high purity aluminum compounds, in particular high purity alumina (HPA) and high purity aluminum salts. [Background technology]
[0002] The following discussion of the background to the present invention is intended to facilitate an understanding of the present invention. However, it should be understood that the discussion is not an acknowledgement or admission that any of the material referred to was published, publicly known, or part of the common general knowledge as of the priority date of the application.
[0003] The US Bureau of Mines (USBM) process for producing high purity alumina from alumina clay has been known since the 1940s. The process consists of multiple steps, which can be summarized as beneficiation, calcination to produce metakaolin, leaching in HCl, two or more successive precipitation and redissolution steps with HCl sparging, and finally calcination to alumina.
[0004] Several variations of the USBM process have been published. For example, US Patent No. 9,382,600 describes leaching of aluminum-containing material with hydrochloric acid to obtain an eluate, which is then reacted with HCl gas to precipitate aluminum chloride. The aluminum chloride precipitate is separated and then converted to alumina by calcination. The gaseous hydrogen chloride evolved during calcination is recycled for use as a leaching agent in the leaching step.
[0005] This process has numerous unit operations and incurs significant capital and operating costs, in particular the need to recycle dry hydrogen chloride gas significantly increases the cost of the process as do the power, materials of construction, and installation of a gas trap during final calcination.
[0006] Many aluminum-containing materials, such as alumina ores, contain significant metal impurities, such as Fe, K, Mg, Na, Ca, Mn, Ba, Zn, Li, Sr, V, Ni, Cr, Pb, Cu, Co, Sb, As, B, Sn, Be, Mo, or mixtures thereof. The production of high purity aluminum compounds from such materials is necessarily complicated by multiple purification steps to successively remove the metal impurities from the aluminum-containing eluate. Such purification steps may include stepwise precipitation of the metal impurities as metal hydroxides by addition of base, followed by separation of a reduced metal impurity aluminum-containing liquid, and / or successive crystallizations, redissolutions, and recrystallizations to further reduce the metal impurities from the aluminum-containing compound.
[0007] WO 2008 / 141423 describes a process for the extraction of aluminum from argillite, an alumina ore containing iron. The argillite is first roasted at a temperature above 550 °C for a period of about 1 to 2 hours. The pretreated argillite is then leached with concentrated hydrochloric acid at a temperature close to the boiling point of the slurry. Iron is subsequently removed from the resulting leachate by increasing the pH to at least 10 by adding NaOH or KOH to precipitate the iron remaining in the solution and other metals except alkali metals, e.g. Na or K. Aluminum may be extracted from the iron-reduced solution by solvent extraction with Cyanex 272, with pH adjustment carried out by a regulating loop controlling the NaOH addition. Complexed aluminum is then recovered by back extraction with hydrochloric acid. The recovered aluminum-rich raffinate is free of iron, but has a composition of Ca, Mg, Na and K above 7%. Further purification to >92.81% is achieved after precipitation of Al(OH)3 aluminum hydroxide, followed by a recrystallization step, but it is not clear that this method will produce what the current market demands for 99.99% purity.
[0008] The methods described herein seek to alleviate some of the problems mentioned above. Summary of the Invention
[0009] The present disclosure provides methods for producing high purity alumina (HPA) and / or high purity aluminum salts from soluble aluminum-containing materials.
[0010] One aspect of the present disclosure is a method for producing high purity alumina (HPA) from an aluminum-containing material, comprising the steps of: Providing an aluminum-containing solution of an aluminum-containing material; selectively extracting aluminum from the aluminum-containing solution by liquid-liquid or liquid-solid extraction to obtain an aluminum-enriched liquid or an aluminum-loaded ion exchange resin; scrubbing the aluminum-enriched liquid or the aluminum-loaded ion exchange resin with an aqueous solution to remove metal impurities therefrom, thereby producing a metal impurity-reduced aluminum-enriched liquid or a metal impurity-reduced aluminum-enriched solid phase; stripping aluminum from the metal impurities-reduced aluminum-rich liquid or the metal impurities-reduced aluminum-rich solid phase by contacting said liquid or said solid phase with an acidic aqueous solution to produce an aluminum-rich aqueous solution; precipitating and separating an aluminum precipitate from the aluminum-rich aqueous solution; calcining the separated aluminum precipitate to produce HPA; The present invention provides a method comprising:
[0011] Another aspect of the present disclosure is a method for producing high purity aluminum salts from an aluminum-containing material, comprising the steps of: Providing an aluminum-containing solution of an aluminum-containing material; Selectively extracting aluminum from the aluminum-containing solution by liquid-liquid or liquid-solid extraction to obtain an aluminum-enriched liquid or aluminum-enriched solid phase; scrubbing the aluminum-enriched liquid or the aluminum-loaded ion exchange resin with an aqueous solution to remove metal impurities therefrom, thereby producing a metal impurity-reduced aluminum-enriched liquid or a metal impurity-reduced aluminum-enriched solid phase; stripping aluminum from the metal impurities-reduced aluminum-rich liquid or metal impurities-reduced aluminum-rich solid phase by contacting said liquid or said phase with an acidic aqueous solution to produce an aluminum-rich aqueous solution; crystallizing and isolating high purity aluminum salts from the aluminum-rich aqueous solution; The present invention provides a method comprising:
[0012] In one embodiment, the step of preparing an aluminium-containing solution of the aluminium-containing material may comprise dissolving the aluminium-containing material in an acid and separating the resulting aluminium-containing solution from remaining insoluble material.
[0013] In another embodiment, the step of preparing an aluminium-containing solution of an aluminium-containing material may comprise dissolving the aluminium-containing material in water and separating the resulting aluminium-containing solution from remaining insoluble material.
[0014] In one embodiment, the step of selectively extracting aluminum from an aluminum-containing solution by liquid-liquid extraction comprises reacting the aluminum-containing solution with an extractant that is selective for aluminum (an "aluminum extractant").
[0015] The aluminum extractant may comprise one or more organophosphorus compounds, in particular organic derivatives of phosphoric acid, phosphonic acid, phosphinic acid or dithiophosphinic acid, optionally in combination with a carboxylic acid, a ketoxime or an aldoxime compound. The aluminum extractant may be present in an organic liquid phase that is immiscible with the aluminum-containing solution, whereby the aluminum extractant reacts with the aluminum-containing solution to transfer aluminum from the aluminum-containing solution to the organic liquid phase and produce an aluminum-rich liquid.
[0016] In one embodiment, the step of selectively extracting aluminum from an aluminum-containing solution by liquid-solid extraction comprises contacting the aluminum-containing solution with an ion exchange resin having selectivity for aluminum relative to monovalent or divalent cations. The ion exchange resin may comprise a strong acid cation resin or a weak acid cation resin.
[0017] In one embodiment, scrubbing the aluminum-rich organic liquid includes contacting the aluminum-rich organic liquid with an aqueous scrub solution to transfer trace metal impurities to the aqueous scrub solution to produce an impurity-reduced aluminum-rich organic liquid phase and an impurity-rich aqueous phase.
[0018] The aqueous scrubbing solution may be a dilute acid or an aqueous solution of aluminum that is substantially free of impurities. In this regard, the aqueous scrubbing solution may include a bleed stream of aluminum-rich aqueous solution obtained by stripping an aluminum-bearing organic liquid phase.
[0019] In one embodiment, the step of stripping the metal impurities-reduced aluminum-rich liquid or metal impurities-reduced aluminum-rich solid phase comprises contacting said liquid or solid phase with an acidic aqueous solution having a pH of 3 or less.
[0020] In one embodiment, the step of crystallizing the high purity aluminum salt from the aluminum-rich solution comprises evaporating sufficient solvent from the aluminum-rich solution to exceed the solubility product of the high purity aluminum salt.
[0021] In one embodiment, the step of precipitating an aluminum precipitate from an aluminum-rich solution comprises increasing the pH of the solution to a range of 4 to 11. Increasing the pH of the solution may be accomplished by adding a base to the solution, in particular by adding aqueous ammonia, NH4OH.
[0022] In one embodiment, the aluminum precipitate comprises aluminum oxyhydroxide, an AlOOH compound.
[0023] In one embodiment, the aluminum precipitate comprises aluminum hydroxide, an Al(OH)3 compound.
[0024] In one embodiment, the precipitating step may be carried out at elevated temperature and optionally at elevated pressure, hi another embodiment, the precipitating step may be maintained at elevated temperature and optionally at elevated pressure for between 15 minutes and 48 hours.
[0025] The step of calcining the aluminum precipitate may be carried out at a temperature between 300° C. and 1400° C. In particular, the calcination step may be carried out in two stages, a first stage at a first temperature for a period sufficient to drive off the water of crystallization from the aluminum precipitate, and a second stage at a temperature higher than the first temperature for a period sufficient to convert the aluminum precipitate to corundum (α-Al2O3), β-alumina or other alumina polymorphs.
[0026] In some embodiments of the present disclosure, the aluminum-containing solution may contain one or more metal impurities, in particular iron. In certain of these embodiments, the method may further include separating the one or more metal impurities from the aluminum-containing solution prior to selectively extracting aluminum from the aluminum-containing solution.
[0027] In one embodiment, the further step of separating one or more metal impurities from the aluminium-containing solution comprises selectively extracting the one or more metal impurities by liquid-liquid extraction or liquid-solid extraction to obtain an aluminium-containing solution having reduced one or more metal impurities.
[0028] In one embodiment, the step of selectively extracting one or more metal impurities from an aluminum-containing solution by liquid-liquid extraction comprises reacting the aluminum-containing solution with an extractant having selectivity for one or more metal impurities, in particular an extractant having selectivity for iron (the "iron extractant"). The iron extractant may comprise a mixture of di(2-ethylhexyl)phosphoric acid and tributyl phosphate, or tributyl phosphate, or trioctylphosphine oxide, or an alkylamine in its free base form.
[0029] The iron extractant may be present in an organic liquid phase that is immiscible in the aluminum-containing solution, such that reaction of the iron extractant with the aluminum-containing solution transfers one or more metal impurities from the aluminum-containing solution to the organic liquid phase.
[0030] In an alternative embodiment, the step of selectively extracting one or more metal impurities from the aluminium-containing solution by liquid-solid extraction comprises contacting the aluminium-containing solution with an ion exchange resin having selectivity for the one or more metal impurities, in particular for iron.
[0031] Preferred embodiments will now be further described and illustrated, by way of example only, with reference to the accompanying drawings, in which: [Brief description of the drawings]
[0032] [Figure 1] FIG. 1 is a schematic diagram of one embodiment of a method for producing high purity alumina (HPA) from soluble aluminum-containing materials disclosed herein. [Diagram 2]FIG. 1 is a schematic diagram of one embodiment of a method described herein for producing high purity aluminum salts, e.g., aluminum nitrate, from soluble aluminum-containing materials. [Diagram 3] 1 is a graphical representation of the extent of extraction of elements from an aluminum-containing material in an acid leaching step to produce an aluminum-containing solution according to one of the examples described herein. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0033] The present disclosure relates to methods for producing high purity alumina (HPA) and / or high purity aluminum salts from soluble aluminum-containing materials.
[0034] [General terms] Throughout this specification, unless specifically stated otherwise or unless otherwise required by context, reference to a single step, composition of matter, group of steps, or group of composition of matter shall be taken to encompass one and the plurality (i.e., one or more) of that step, composition of matter, group of steps, or group of composition of matter. Thus, as used herein, the singular forms "a," "an," and "the" include plural aspects unless the context dictates otherwise. For example, reference to "a" includes both the singular and more than one, reference to "an" includes both the singular and more than one, reference to "the" includes both the singular and more than one, and so forth.
[0035] Each of the examples of the disclosure described herein may be applied to every other example, mutatis mutandis, unless specifically stated otherwise. The disclosure should not be limited in scope by the specific examples described herein, which are intended for illustrative purposes only. Functionally equivalent products, compositions and methods are clearly within the scope of the disclosure described herein.
[0036] The method steps, methods, and operations described herein should not necessarily be construed as requiring performance in the particular order discussed or illustrated, unless specifically identified as performing a certain order. It should also be understood that additional or alternative steps may be employed.
[0037] When an element or layer is referred to as "on," "engaged with," "connected to," or "bonded to" another element or layer, it can be directly in contact with, engaged with, connected to, or bonded to the other element or layer, or intervening elements or layers may be present. In contrast, when an element is referred to as being "directly on," "directly engaged," "directly connected," or "directly bonded to" another element or layer, there must not be intervening elements or layers. Other words used to describe relationships between elements should be interpreted similarly (e.g., "directly between" as opposed to "between," "directly adjacent" as opposed to "adjacent," etc.).
[0038] Terms such as first, second, third, etc. may be used herein to describe various elements, components, regions, layers, and / or sections, but these elements, components, regions, layers, and / or sections should not be limited by these terms. These terms may only be used to distinguish one element, component, region, layer, or section from another region, layer, or section. Terms such as "first," "second," and other numerical terms, when used herein, do not imply a sequence or order unless clearly indicated by context. Thus, a first element, component, region, layer, or section discussed below can be referred to as a second element, component, region, layer, or section without departing from the teachings of the example embodiments.
[0039] References to descriptions of positions such as below and above should be taken in the context of the illustrated embodiments and should not be taken as limiting the invention to a literal interpretation of the terms, but rather as understood by one of ordinary skill in the art.
[0040] Spatially relative terms, such as "in," "out," "beneath," "below," "lower," "above," and "above," may be used herein for ease of description to describe the relationship of one element or feature illustrated in the figures to another element or feature. Spatially relative terms may be intended to encompass devices in different orientations in use or operation in addition to the orientation depicted in the figures. For example, if a device in the figures is upside down, an element described as "below" or "beneath" the other element or feature would then be oriented "above" the other element or feature. Thus, the exemplary term "below" can encompass both an orientation of above and below. A device may be otherwise oriented (rotated 90 degrees or at other orientations) and the spatially relative descriptors used herein interpreted accordingly.
[0041] The term "and / or", e.g., "X and / or Y", shall be understood to mean either "X and Y" or "X or Y", and shall be taken as providing explicit support in both cases or in either case.
[0042] Throughout this specification, the word "comprise" and variations such as "comprises" or "comprising" are understood to imply the inclusion of a stated element, integer or step, or group of elements, integers or steps, but not the exclusion of any other element, integer or step, or group of elements, integers or steps.
[0043] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which this invention belongs. Although methods and materials similar or equivalent to those described herein can be used to practice or test the present invention, the preferred methods and materials are described below. In case of conflict, the present specification, including definitions, will take precedence. In addition, the materials, methods and examples are only illustrative and are not intended to be limiting.
[0044] The term "about" as used herein means within 5%, more preferably within 1% of a given value or range. For example, "about 3.7%" means 3.5-3.9%, preferably 3.66-3.74%. When the term "about" is in relation to a range of values, e.g., "about X%-Y%", the term "about" is intended to modify both the lower limit (X) and the upper limit (Y) of the recited range. For example, "about 20%-40%" is equivalent to "about 20%-about 40%".
[0045] [Specific terminology] As used herein, the term "high purity alumina" refers to alumina (α-Al2O3, β-Al2O3 or other crystalline polymorphs thereof) having a purity of 99.99% or greater.
[0046] The term "liquid-liquid extraction", also known as solvent extraction, is used to refer to a method of separating chemical compounds or metal complexes based on their relative solubility in two different immiscible liquid phases, usually water (polar) and an organic liquid (non-polar). Typically, to aid in the transfer of the chemical compound or metal complex from the polar phase to the non-polar phase, the two phases are agitated to increase the interfacial surface area between them. The degree to which a substance can transfer from the polar phase to the non-polar phase is known as the partition ratio (K d The partition ratio is referred to as the distribution ratio (distribution ratio) and is equal to the concentration of the substance in the non-polar phase divided by the concentration of the substance in the polar phase. The partition ratio can vary depending on any one or more of several factors, including, but not limited to, temperature, pH, the nature of the polar and non-polar phases, the total concentration of the species in the phase, and the presence of other species in the phase.
[0047] In some specific liquid-liquid extraction systems, an extractant may be used to increase the distribution ratio of a substance in the organic phase. The term "extractant" as used herein refers to a chemical compound that can react with or bind to a substance so that the distribution ratio of the substance is increased. For metal ions, particularly divalent and trivalent metal cations, the extractant may be an organic compound that reacts with the metal cation to form a metal complex that has a higher distribution ratio than the metal ion, thereby assisting in the extraction of the metal ion into the non-polar phase. It will be understood by those skilled in the art that the extractant may further comprise a mixture of two or more chemical compounds that can react with or bind to the metal ion. In particular, the extractant may be a mixture of two or more chemical compounds that have a synergistic improvement in the distribution ratio of the target metal ion or an improvement in the relative distribution ratio of the target metal ion compared to the non-target impurity metal ions.
[0048] The term "selectively extract" as used herein refers to an extraction system (e.g., liquid-liquid extraction) in which the partition ratio for a first substance in the extraction system is sufficiently higher than the respective partition ratios for a second substance in the extraction system such that the first substance is preferentially extracted therein. In general, the separation factor (i.e., the partition coefficient of the first substance divided by the separation coefficient of the second substance) can be greater than 2, greater than 5, greater than 10, greater than 20, greater than 50, greater than 100, greater than 200, greater than 500, or greater than 1000.
[0049] The term "enriched" means having a higher mole percent concentration of the indicated constituent than the stream from which it was originally formed.
[0050] The term "depleted" means having a lower mole percent concentration of the indicated constituent than the stream from which it was originally formed.
[0051] The term "lean" means having a mole percent concentration of the indicated component of less than 5 mole percent, less than 2 mole percent, or less than 1 mole percent.
[0052] As used herein, the term "solubility product" refers to the maximum product between ion concentrations or activities of ionic compounds that can remain in equilibrium with a non-dissolved phase at a known temperature.
[0053] [Method for producing high purity alumina or aluminum salts] Several high purity aluminum salts, or HPAs, can be prepared from a variety of aluminum-containing materials by the methods disclosed herein.
[0054] For example, the aluminum-containing material may be a water-soluble aluminum salt, including, but not limited to, aluminum chloride, aluminum nitrate, or aluminum sulfate.
[0055] Alternatively, the aluminium-containing material may be an acid-soluble aluminium-containing material, including but not limited to oxides, hydroxides and oxyhydroxides of aluminium, aluminosilicate minerals or aluminium-containing slags. It will be appreciated that the acid-soluble aluminium-containing material may be a by-product or residue produced by different processes.
[0056] Suitable examples of oxides, hydroxides and oxyhydroxides of aluminum can be corundum, boehmite, diaspore, bayerite, doyleite, nordstrandite and gibbsite.
[0057] Suitable examples of aluminosilicate minerals can be clay minerals, in particular dickite, halloysite and kaolin.
[0058] The aluminum-containing solution may be prepared by dissolving a water-soluble aluminum salt in water.
[0059] Alternatively, the aluminum-containing solution may be prepared by dissolving the acid-soluble aluminum material in an acid. The acid may be a strong mineral acid, such as hydrochloric acid, nitric acid or sulfuric acid. It will be understood by those skilled in the art that dissolution conditions vary depending on the nature of the acid-soluble aluminum material, but can be easily determined by systematically varying the ratio of the acid-soluble aluminum material to the acid, the acid concentration, temperature, agitation, pressure and time.
[0060] Any remaining insoluble material can be separated from the aluminum-containing solution by filtration or other well-understood separation techniques.
[0061] In some embodiments, the aluminum-containing solution may have an aluminum concentration of at least 1 g / L, or at least 5 g / L, or at least 10 g / L, or at least 20 g / L, or at least 40 g / L, or at least 60 g / L, or may be saturated in aluminum concentration. It will be appreciated that the state of saturation may depend on one or more factors, including, but not limited to, the temperature and pH of the aluminum-containing solution.
[0062] In some embodiments, the aluminum concentration of the aluminum-containing solution may be between 1 g / L and saturation, or between 2 g / L and saturation, or between 5 g / L and saturation, or between 10 g / L and saturation, or between 20 g / L and saturation, or between 40 g / L and saturation, or between 60 g / L and saturation.
[0063] [Removal of one or more metal impurities, especially iron] In some embodiments, the aluminum-containing solution may contain one or more metal impurities, such as Fe, K, Mg, Na, Ca, Mn, Ba, Zn, Li, Sr, V, Ni, Cr, Pb, Cu, Co, Sb, As, B, Sn, Be, Mo. The ratio of total metals (excluding Al) to Al in the aluminum-containing solution may be 1:1, 1:2, 1:5, 1:10, 1:20, 1:50, 1:100, 1:200, 1:500, 1:1000, 1:2000, 1:5000 or more than 1:5000. It may be advantageous to separate one or more metal impurities, especially iron, before selectively extracting aluminum from the aluminum-containing solution.
[0064] The step of separating iron from the aluminum-containing solution comprises selectively extracting iron from the aluminum-containing solution by liquid-liquid extraction or liquid-solid extraction to obtain an iron-reduced aluminum-containing solution.
[0065] In some embodiments, the aluminum-containing solution may be reacted with an iron extractant present in an immiscible organic liquid phase, where the iron extractant is selective for iron. Reacting the iron extractant with the aluminum-containing solution transfers iron from the aluminum-containing solution to the organic liquid phase to produce an iron-rich organic liquid and an iron-reduced aluminum-containing solution.
[0066] The iron extractant may include a mixture of di(2-ethylhexyl)phosphate and tributyl phosphate, or tributyl phosphate, or trioctylphosphine oxide, or an alkylamine in its free base form. Suitable alkylamines include, but are not limited to, primary, secondary, and tertiary alkylamines, such as Alamine 336, which is a mixture of tri-C8-C10 amines.
[0067] The iron extractant may be present in the organic liquid phase at a concentration of greater than 0.1%, greater than 0.5%, greater than 1%, greater than 2%, greater than 3%, greater than 4%, greater than 5%, greater than 7%, greater than 10%, greater than 15%, greater than 20%, greater than 30%, greater than 40%, greater than 50%, greater than 60%, greater than 70%, greater than 80%, greater than 90%, or even greater than 95% by volume.
[0068] The iron extractant may be present in the organic liquid phase at a concentration of between 0.5% and 1% by volume, or between 0.5% and 2% by volume, or between 0.5% and 3% by volume, or between 0.5% and 4% by volume, or between 0.5% and 5% by volume, or between 0.5% and 7% by volume, or between 0.5% and 10% by volume, or between 0.5% and 15% by volume, or between 0.5% and 20% by volume, or between 0.5% and 30% by volume, or between 0.5% and 40% by volume, or between 0.5% and 50% by volume, or between 0.5% and 60% by volume, or between 0.5% and 70% by volume, or between 0.5% and 80% by volume, or between 0.5% and 90% by volume, or between 0.5 and 95% by volume.
[0069] The organic liquid phase may include one or more organic solvents that are immiscible with the aqueous phase. In particular, the organic liquid phase may include one or more aliphatic hydrocarbons. Aliphatic hydrocarbons are organic compounds that have saturated, long straight, branched or cyclic hydrocarbon chains. Exemplary aliphatic hydrocarbons are kerosene, hexane and heptane.
[0070] In some embodiments, the method further comprises adding a phase modifier to the solvent to prevent the formation of three phases during the liquid-liquid extraction process. The phase modifier may comprise a surfactant or a co-solvent. Suitable examples of these modifiers include, but are not limited to, isodecanol (1-decanol, CAS 112-30-1, C 10 H 22In embodiments where the iron extractant comprises di(2-ethylhexyl)phosphoric acid and tributyl phosphate, it will be appreciated that the tributyl phosphate may also act as a phase modifier.
[0071] In an embodiment, the phase modifier may be present in the organic liquid phase at a concentration of greater than 1 vol.%, greater than 2.5 vol.%, greater than 5 vol.%, greater than 7.5 vol.%, greater than 10 vol.%, greater than 15 vol.%, or greater than 20 vol.%.
[0072] In one embodiment, the phase modifier may be present in the organic liquid phase at a concentration of 1-50%, 2.5-50%, 5-50%, 7.5-50%, 10-50%, or 15-50% by volume.
[0073] The step of contacting the aqueous phase with the organic phase may be achieved by any method known in the art for mixing a first liquid with a second immiscible liquid. Thus, a mixer-settler may be used, and the step of contacting may be performed or repeated until the desired amount of iron is transferred from the aqueous phase to the organic phase. The number of extraction stages, e.g., the number of consecutive solvent extractions actually performed between the aluminum-containing solution and the organic liquid phase, depends on the excess free acid present in the aluminum-containing solution, the amount of iron present, and the efficiency of the transfer in the contact between the two liquid phases. Other suitable extraction equipment that may be used includes, but is not limited to, mixer-settlers and centrifugal extractors. Separation of the organic and aqueous phases may be achieved by decantation or by using a centrifuge, the latter method being generally more efficient.
[0074] Advantageously, the iron extractant is selective for iron, but several other transition metal ions, such as Mn, Zn, V, Ni, Cr, Pb, Cu, Co, Sb, As, Sn and Mo, may also be co-extracted with iron.
[0075] In an alternative embodiment, the aluminum-containing solution may be contacted with an ion exchange resin that is selective for iron relative to aluminum and other divalent and monovalent cations to reduce iron from the aluminum-containing solution.
[0076] The ion exchange resin may be selected from the group including strong acid cation resins, weak acid cation resins.
[0077] The ion exchange resin can be contacted with the aluminum-containing solution using either static or dynamic methods. For example, in static methods, the ion exchange resin can be contained using one or more vertical columns through which the aluminum-containing solution can be eluted to extract iron from the solution.
[0078] In one form of the invention, the ion exchange resin may be neutralized prior to contact with the iron-containing aluminum solution by eluting it with an alkaline solution, which may be a dilute solution of sodium hydroxide, potassium hydroxide, lithium hydroxide, aqueous ammonia, calcium hydroxide, magnesium hydroxide or mixtures thereof.
[0079] Selective extraction of aluminum from aluminum-containing solutions (liquid-liquid extraction) After the optional removal of iron from the aluminum-containing solution, the method may include a step of selectively extracting aluminum from the aluminum-containing solution by liquid-liquid extraction, in particular by solvent extraction. The aluminum-containing solution may be reacted with an aluminum extractant present in an immiscible organic liquid phase, where the aluminum extractant has selectivity for aluminum. Reacting the aluminum extractant with the aluminum-containing solution transfers aluminum from the aluminum-containing solution to the organic liquid phase to produce an aluminum-rich organic liquid.
[0080] It will be appreciated that several stages of extraction may be required to recover most of the aluminum from the aluminum-containing solution.
[0081] The aluminium extractant may comprise one or more organophosphorus compounds, in particular organic derivatives of phosphoric acid, phosphonic acid, phosphinic acid or dithiophosphinic acid. The organophosphorus compound or compounds may conveniently be in a liquid phase under ambient conditions and may be easily combined with an organic liquid phase.
[0082] Suitable examples of organophosphorus extractants include, but are not limited to, bis(2,4,4-trimethylpentyl)phosphonic acid, also known as Cyanex 272 (CAS number 83411-71-6), 2-ethylhexylphosphonic acid mono-2-ethylhexyl ester, also known as Ionquest 801 (CAS number 14802-03-0), bis(2,4,4-trimethylpentyl)dithiophosphinic acid, also known as Cyanex 301 (CAS number 107667-02-7), Cyanex 302 (CAS number 132767-86-3), also known as bis(2,4,4-trimethylpentyl)monothiophosphinic acid, bis(2-ethylhexyl) hydrogen phosphate (BEHHP), bis(2-ethylhexyl)phosphate (BEHPA), bis(2-ethylhexyl)phosphate (BEHP), bis(2-ethylhexyl)hydrophosphate (BEHHPA), di-(2-ethylhexyl)phosphate (DEHPA) (C8H 17 O) 2PO2H (CAS number 298-07-7).
[0083] In some embodiments, the extractant may further comprise a carboxylic acid, a ketoxime, or an aldoxime compound.
[0084] The extractant may be present in the organic liquid phase in a concentration of greater than 0.1%, greater than 0.5%, greater than 1%, greater than 2%, greater than 3%, greater than 4%, greater than 5%, greater than 7%, greater than 10%, greater than 15%, greater than 20%, greater than 30%, greater than 40%, greater than 50%, greater than 60%, greater than 70%, greater than 80%, greater than 90%, or even greater than 95% by volume.
[0085] The extractant may be present in the organic liquid phase in a concentration of between 0.5% and 1% by volume, or between 0.5% and 2% by volume, or between 0.5% and 3% by volume, or between 0.5% and 4% by volume, or between 0.5% and 5% by volume, or between 0.5% and 7% by volume, or between 0.5% and 10% by volume, or between 0.5% and 15% by volume, or between 0.5% and 20% by volume, or between 0.5% and 30% by volume, or between 0.5% and 40% by volume, or between 0.5% and 50% by volume, or between 0.5% and 60% by volume, or between 0.5% and 70% by volume, or between 0.5% and 80% by volume, or between 0.5% and 90% by volume, or between 0.5 and 95% by volume.
[0086] As indicated above, the aluminum extractant may comprise a binary mixture of two compounds selected from the group including Cyanex 272, Cyanex 301, Cyanex 302, Ionquest 801, D2EHPA, carboxylic acids, ketoximes, aldoximes. Examples of suitable carboxylic acids include, but are not limited to, highly branched tertiary carboxylic acids such as neodecanoic acid (also known as Versatic Acid 10). Suitable ketoximes and aldoximes include, but are not limited to, hydroxyaryl ketoximes and hydroxyaryl aldoximes.
[0087] The ratio of the two compounds present in a binary mixture may be 0.1:99.9%, 0.5:99.5%, 1.0:99.0%, 2.0:98.0%, 5.0:95.0%, 10.0:90.0%, 20.0:80.0%, 30.0:70.0%, 40.0:60.0%, 50.0:50.0%, 60.0:40.0%, 70.0:30.0%, 80.0:20.0%, 90.0:10.0%, 95.0:5.0%, 98.0:2.0%, 99.0:1.0%, 99.5:0.5% or 99.9:0.1%.
[0088] Binary mixtures include Cyanex 272 and Cyanex 301, Cyanex 272 and Cyanex 302, Cyanex 272 and Ionquest 801, Cyanex 272 and D2EHPA, Cyanex 272 and carboxylic acid, Cyanex 272 and ketoxime, Cyanex 272 and aldoxime, Cyanex 301 and Cyanex 302, Cyanex 301 and Ionquest 801, Cyanex 301 and D2EHPA, Cyanex 301 and carboxylic acid, Cyanex 301 and ketoxime, Cyanex 301 and aldoxime, Cyanex 302 and Ionquest 801, Cyanex 302 and D2EHPA, Cyanex 302 and carboxylic acid, Cyanex 302 and ketoxime, Cyanex 302 and an aldoxime, IonQuest 801 and D2EHPA, IonQuest 801 and a carboxylic acid, IonQuest 801 and a ketoxime, IonQuest 801 and an aldoxime, D2EHPA and a carboxylic acid, D2EHPA and a ketoxime, D2EHPA and an aldoxime, a carboxylic acid and a ketoxime, a carboxylic acid and an aldoxime, a ketoxime and an aldoxime.
[0089] As indicated above, the aluminum extract may comprise a ternary mixture of three compounds selected from the group of compounds including Cyanex 272, Cyanex 301, Cyanex 302, Ionquest 801, D2EHPA, carboxylic acids, ketoximes, and aldoximes.
[0090] Ternary mixtures are Cyanex 272 and Cyanex 301 and Cyanex 302, Cyanex 272 and Cyanex 301 and IonQuest 801, Cyanex 272 and Cyanex 301 and D2EHPA, Cyanex 272 and Cyanex 301 and carboxylic acid, Cyanex 272 and Cyanex 301 and aldoxime, Cyanex 272 and Cyanex 301 and ketoxime, Cyanex 272 and Cyanex 302 and IonQuest 801, Cyanex 272 and Cyanex 302 and D2EHPA, Cyanex 272 and Cyanex 302 and carboxylic acid, Cyanex 272 and Cyanex 302 and aldoxime, Cyanex 272 and Cyanex 302 and ketoxime, Cyanex 272 and IonQuest 801 and D2EHPA, Cyanex 272 and IonQuest 801 and carboxylic acid, Cyanex 272 and IonQuest 801 and aldoxime, Cyanex 272 and IonQuest 801 and ketoxime, Cyanex 272 and D2EHPA and carboxylic acid, Cyanex 272 and D2EHPA and aldoxime, Cyanex 272 and D2EHPA and ketoxime, Cyanex 272 and carboxylic acid and aldoxime, Cyanex 272 and carboxylic acid and ketoxime, Cyanex 272 and aldoxime and ketoxime, Cyanex 301 and Cyanex 302 and IonQuest 801, Cyanex 301 and Cyanex 302 and D2EHPA, Cyanex 301 and Cyanex 302 and carboxylic acid, Cyanex 301 and Cyanex 302 and aldoxime, Cyanex 301 and Cyanex 302 and ketoxime, Cyanex 301 and IonQuest 801 and D2EHPA, Cyanex 301 and IonQuest 801 and carboxylic acid, Cyanex 301 and IonQuest 801 and aldoxime, Cyanex 301 and IonQuest801 and ketoxime, Cyanex 301 and D2EHPA and carboxylic acid, Cyanex 301 and D2EHPA and aldoxime, Cyanex 301 and D2EHPA and ketoxime, Cyanex 301 and carboxylic acid and aldoxime, Cyanex 301 and carboxylic acid and ketoxime, Cyanex 301 and aldoxime and ketoxime, Cyanex 302 and IonQuest 801 and D2EHPA, Cyanex 302 and IonQuest 801 and carboxylic acid, Cyanex 302 and IonQuest 801 and aldoxime, Cyanex 302 and IonQuest 801 and ketoxime, Cyanex 302 and D2EHPA and carboxylic acid, Cyanex 302 and D2EHPA and aldoxime, Cyanex 302 and D2EHPA and ketoxime, Cyanex 302 and carboxylic acid and aldoxime, Cyanex 302 and carboxylic acid and ketoxime, Cyanex 302 and aldoxime and ketoxime, IonQuest 801 and D2EHPA and carboxylic acid, IonQuest 801 and D2EHPA and aldoxime, IonQuest 801 and D2EHPA and ketoxime, IonQuest 801 and carboxylic acid and aldoxime, IonQuest 801 and carboxylic acid and ketoxime, IonQuest 801 and aldoxime and ketoxime, D2EHPA and carboxylic acid and aldoxime, D2EHPA and carboxylic acid and ketoxime, D2EHPA and aldoxime and ketoxime, carboxylic acid and aldoxime and ketoxime.
[0091] In a further embodiment, the aluminum extractant may comprise a mixture of higher quaternary compounds in the group including Cyanex 272, Cyanex 301, Cyanex 302, IonQuest 801, D2EHPA, carboxylic acids, ketoximes or aldoximes.
[0092] The organic liquid phase may include one or more organic solvents that are immiscible with the aqueous phase. In particular, the organic liquid phase may include one or more aliphatic hydrocarbons. Aliphatic hydrocarbons are organic compounds that have saturated, long straight, branched or cyclic hydrocarbon chains. Exemplary aliphatic hydrocarbons are kerosene, hexane and heptane.
[0093] In some embodiments, the method further comprises adding a phase modifier to the solvent to prevent the formation of three phases during the liquid-liquid extraction. The phase modifier may comprise a surfactant or a co-solvent. Suitable examples of phase modifiers include, but are not limited to, isodecanol (1-decanol, CAS 112-30-1, C 10 H 22 O), especially tributyl phosphate (TBP, CAS 126-73-8, C 12 H 27 O4P) are examples.
[0094] In an embodiment, the phase modifier may be present in the organic liquid phase at a concentration of greater than 1 vol.%, greater than 2.5 vol.%, greater than 5 vol.%, greater than 7.5 vol.%, greater than 10 vol.%, greater than 15 vol.%, or greater than 20 vol.%.
[0095] In one embodiment, the phase modifier may be present in the organic liquid phase at a concentration of 1-50%, 2.5-50%, 5-50%, 7.5-50%, 10-50%, or 15-50% by volume.
[0096] The solvent extraction step may be carried out at a temperature below the boiling point of the organic liquid phase. In various embodiments, the solvent extraction step may be carried out at a temperature between ambient temperature and 30°C, between ambient temperature and 35°C, between ambient temperature and 40°C, between ambient temperature and 45°C, between ambient temperature and 50°C, between ambient temperature and 55°C, or between ambient temperature and 60°C.
[0097] The organic liquid phase containing the aluminum extractant may be neutralized before reacting it with the aluminum-containing solution. The organic liquid phase containing the aluminum extractant may be mixed with an alkaline solution, in particular sodium hydroxide, potassium hydroxide, lithium hydroxide or aqueous ammonia. Alternatively, the organic liquid phase containing the extractant may be mixed with an alkaline suspension, in particular calcium hydroxide, lime, hydrated lime, magnesium hydroxide or magnesium oxide.
[0098] Alternatively, if the organic liquid phase has not been previously neutralized, it may be necessary to add an alkaline solution to maintain the desired pH, especially pH<4. The concentration of the alkaline solution should not be sufficient to induce precipitation of Al in the aqueous phase. As one skilled in the art will recognize, this is a matter of trial and error and will be affected by the strength of mixing of the aqueous and organic liquid phases.
[0099] During the extraction of aluminum, neutralization of protons exchanged from the extractant can be accomplished by adding ammonia solution between loading stages to achieve the desired pH at each stage. As those skilled in the art will recognize, protons can also be partially or completely pre-neutralized by directly contacting the metal-reduced and stripped organics with ammonia solution, which neutralizes the protons with ammonia, effectively forming the ammonium salt of D2EHPA. The ammonium salt of D2EHPA is then reacted with the loaded aluminum solution, exchanging the aluminum ions for ammonium ions with minimal pH change in the aqueous phase. Pre-neutralization may also be accomplished using other bases, including but not limited to NaOH, KOH, MgO, Mg(OH)2, Ca(OH)2, to form the relevant D2EHPA salt. In the most preferred form, ammonia is used as the neutralizing agent to limit the introduction of alkali metal or alkaline earth metal impurities in the system.
[0100] [Removal of trace metal impurities] Trace metal impurities, especially alkali metals such as Li, Na and K, and alkaline earth metals such as Be, Mg and Ca, may still remain in the aluminum-rich organic liquid phase. If the objective is to obtain 99.99% pure alumina or aluminum salt, the removal of such impurities is important. Trace metal impurities can be removed by contacting the aluminum-rich organic liquid with an aqueous scrub solution to transfer trace metal impurities to the aqueous scrub solution, thereby producing an impurity-reduced aluminum-rich organic liquid phase and an impurity-rich aqueous phase.
[0101] The aqueous scrubbing solution may be a dilute acid. In particular, the acid may be selected from the group including sulfuric acid, hydrochloric acid, nitric acid, and phosphoric acid. As one skilled in the art will recognize, the optimum pH for impurity removal will vary depending on the extractant used.
[0102] In some embodiments, the impurities-rich aqueous phase may have a pH of less than 4. The pH of the impurities-rich aqueous phase may be between 0.5 and 4, between 0.5 and 3, between 0.5 and 2, or between 0.5 and 1.
[0103] Alternatively, the aqueous scrubbing solution may comprise an aqueous solution of aluminum that is substantially free of impurities. In this regard, the aqueous scrubbing solution may comprise a bleed stream of aluminum-rich aqueous solution obtained by stripping an aluminum-loaded organic liquid phase (described below).
[0104] The aluminum concentration in the aqueous scrub solution can be between 0.1 g / L and the saturation concentration of aluminum precipitate or aluminum salts ("saturation"), between 1.0 g / L and saturation, between 5.0 g / L and saturation, between 10 g / L and saturation, between 25 g / L and saturation, between 50 g / L and saturation, between 75 g / L and saturation, between 100 g / L and saturation, between 150 g / L and the saturation of the relevant salt.
[0105] [Selective extraction of aluminum from aluminum-containing solutions (liquid-solid extraction)] Alternatively, aluminum may be extracted from the aluminum-containing solution by contacting the aluminum-containing solution with an ion exchange resin having selectivity for aluminum compared to monovalent or divalent cations. The ion exchange resin may comprise a strong acid cation resin or a weak acid cation resin.
[0106] The ion exchange resin can be contacted with the aluminum-containing solution using either static or dynamic methods. For example, in static methods, the ion exchange resin can be contained using one or more vertical columns through which the aluminum-containing solution can be eluted, whereupon the aluminum ions exchange with and bind to the cations on the ion exchange resin, resulting in an aluminum-loaded resin.
[0107] Prior to elution with the aluminum-containing solution, the ion exchange resin may be neutralized by eluting it with an alkaline solution, which may be a dilute solution of sodium hydroxide, potassium hydroxide, lithium hydroxide, aqueous ammonia, calcium hydroxide, magnesium hydroxide or mixtures thereof.
[0108] [Removal of trace metal impurities] Trace amounts of monovalent or divalent metal impurities, particularly alkali metals such as Li, Na and K, and alkaline earth metals such as Mg and Ca, also loaded on the resin, may be removed from the resin by eluting the aluminum-loaded resin with an aqueous scrubbing solution to transfer the trace metal impurities to the aqueous scrubbing solution, thereby producing an impurity-reduced aluminum-rich organic liquid phase and an impurity-rich aqueous phase.
[0109] The aqueous scrubbing solution may be a dilute acid. In particular, the acid may be selected from the group including sulfuric acid, hydrochloric acid, nitric acid, and phosphoric acid. As one skilled in the art will recognize, the optimum pH for impurity removal will vary depending on the extractant used.
[0110] In some embodiments, the impurities-rich aqueous phase may have a pH of less than 4. The pH of the impurities-rich aqueous phase may be between 0.5 and 4, between 0.5 and 3, between 0.5 and 2, or between 0.5 and 1.
[0111] Alternatively, the aqueous scrubbing solution may comprise an aqueous solution of aluminum that is substantially free of impurities. In this regard, the aqueous scrubbing solution may comprise a bleed stream of aluminum-rich aqueous solution obtained by stripping an aluminum-loaded organic liquid phase (described below).
[0112] The aluminum concentration in the aqueous scrub solution can be between 0.1 g / L and the saturation concentration of aluminum precipitate or aluminum salts ("saturation"), between 1.0 g / L and saturation, between 5.0 g / L and saturation, between 10 g / L and saturation, between 25 g / L and saturation, between 50 g / L and saturation, between 75 g / L and saturation, between 100 g / L and saturation, between 150 g / L and the saturation of the relevant salt.
[0113] Stripping aluminum from aluminum-rich liquids or aluminum-loaded resins. The methods described herein also include the step of stripping aluminum from the aluminum-rich liquid or aluminum-loaded resin, respectively, by contacting the aluminum-rich liquid or aluminum-loaded resin with an acidic aqueous solution to produce an aluminum-rich aqueous solution.
[0114] The acid may be selected from the group of strong mineral acids, including, but not limited to, hydrochloric acid, sulfuric acid, nitric acid, phosphoric acid, or mixtures thereof. The acid may be selected from the group of weak acids, whose anions form soluble complex ions with aluminum. The group of weak acids includes, but is not limited to, citric acid, oxalic acid, acetic acid, gluconic acid, saccheric acid, and malonic acid.
[0115] Advantageously, in embodiments producing a high purity aluminum salt, the acid used to prepare the acidic aqueous solution may correspond to the desired salt, for example, if the high purity aluminum salt is aluminum sulfate, the acid may be sulfuric acid, if the high purity aluminum salt is aluminum nitrate, the acid may be nitric acid, if the high purity aluminum salt is aluminum chloride, the acid may be hydrochloric acid.
[0116] Alternatively, in embodiments producing high purity alumina, the acid may be nitric acid, hydrochloric acid or a weak acid.
[0117] The dilute aqueous aluminum solution may contain between 0.1 g / L and 10 g / L of free acid, between 0.1 g / L and 20 g / L of free acid, between 0.1 g / L and 30 g / L of free acid, between 0.1 g / L and 40 g / L of free acid, between 0.1 g / L and 50 g / L of free acid, between 0.1 g / L and 75 g / L of free acid, between 0.1 g / L and 100 g / L of free acid, between 0.1 g / L and 150 g / L of free acid, or between 0.1 g / L and 200 g / L of free acid.
[0118] The pH of the aluminium-rich aqueous solution obtained after contact with the dilute aluminium aqueous solution may be less than 3, in particular between 0 and 3, between 0.5 and 3, between 1.0 and 3, between 1.5 and 3, between 2.0 and 3, between 2.5 and 3, between 0 and 2, between 0.5 and 2, between 1.0 and 2 or between 1.5 and 2.
[0119] [Crystallization and separation of high-purity aluminum salts] In some embodiments, the methods described herein include the step of crystallizing and isolating high purity aluminum salts from an aluminum-rich aqueous solution.
[0120] In general, the aluminum-rich aqueous solution may be heated to reduce the volume of water to such an extent that the solubility product of the relevant salt is exceeded and the salt crystallizes out of solution. Heating may be performed under reduced pressure. As one skilled in the art will recognize, the conditions for evaporation depend on the salt content of the solution, the maximum solubility of the salt, and can be determined by straightforward experimental work.
[0121] The resulting high purity aluminum salt crystals may be separated from the mother liquor by filtration, decantation, centrifugation, and other conventional separation techniques that will be well understood by those skilled in the art. It will be appreciated that the separated high purity aluminum salt may be washed one or more times and dried.
[0122] [Aluminum Precipitate and Separation] In an alternative embodiment, the methods described herein include the step of crystallizing and isolating aluminum hydroxide or aluminum oxyhydroxide compounds from an aluminum-rich aqueous solution.
[0123] The aluminum hydroxide or aluminum oxyhydroxide compound may be precipitated from the solution by increasing the pH of the solution to a range of 4-11, 5-10, 6-9, especially 7-8.
[0124] As one of ordinary skill in the art will recognize, aluminum is amphoteric and soluble in both acid and alkaline solutions. Therefore, the optimum pH is determined by the amount of tetrahydroaluminate, Al(OH)4 - The pH is below which solubility increases due to the formation of
[0125] The pH of the solution may be increased by adding a base to the solution. The base may be selected from the group including sodium hydroxide, potassium hydroxide, lithium hydroxide, calcium oxide, calcium hydroxide, ammonia, magnesium hydroxide, magnesium oxide. In particular, the pH of the solution may be increased by adding aqueous ammonia, NH4OH, to the solution.
[0126] Depending on the reaction conditions, the precipitation step may produce a crystalline product, particularly aluminum hydroxide, or aluminum oxyhydroxide, such as boehmite, AlOOH.
[0127] The precipitation step may be carried out at elevated temperatures, in particular at temperatures above 30° C., above 40° C., above 50° C., above 60° C., above 70° C., above 80° C., above 90° C., above 100° C., or up to the boiling point of the aluminium-rich aqueous solution.
[0128] The precipitating step may be carried out at a temperature between 30° C. and the boiling point, between 40° C. and the boiling point, between 50° C. and the boiling point, between 60° C. and the boiling point, between 70° C. and the boiling point, between 80° C. and the boiling point, between 90° C. and the boiling point, or between 100° C. and the boiling point of the aluminium-rich aqueous solution. Pressure may be used to increase the boiling point of the solution by carrying out the precipitating step under hydrothermal conditions.
[0129] As one skilled in the art would recognize, the precipitate may be aged in the mother liquor to form more crystalline phases or to increase the particle size of the resulting precipitate, thereby aiding in solid-liquid separation. It will be appreciated that the mother liquor may be held at the same or similar temperature and at the same or similar pressure as the precipitating step.
[0130] The aging step can vary from 30 minutes to 48 hours depending on various operating conditions. For example, the aging step can be more than 15 minutes, more than 30 minutes, more than 60 minutes, more than 2 hours, more than 4 hours, more than 8 hours, more than 16 hours or more than 24 hours.
[0131] The aging step may have a duration between 15 minutes and 48 hours, between 30 minutes and 48 hours, between 60 minutes and 48 hours, between 2 hours and 48 hours, between 4 hours and 48 hours, between 8 hours and 48 hours, between 12 hours and 48 hours, or between 24 hours and 48 hours.
[0132] As one skilled in the art will recognize, precipitation of aluminum hydroxide compounds may be carried out in an autoclave utilizing elevated pressure to prevent boiling of the aluminum-rich aqueous solution when heated above its boiling point at atmospheric pressure, with optimal conditions readily determined by standard test work protocols.
[0133] The resulting aluminum precipitate may be separated by filtration, decantation, centrifugation, and other conventional separation techniques that will be well understood by those skilled in the art. It will be appreciated that the separated precipitate may be washed one or more times and dried.
[0134] It will be appreciated that the aluminum precipitate produced as described herein may be a marketable product.
[0135] [Caking of precipitate] The method described herein includes the step of calcining the separated aluminum precipitate to produce high purity alumina, Al2O3.
[0136] The calcining step may be carried out by heating the aluminum precipitate to a temperature sufficient to convert the aluminum precipitate to alumina, for example, the aluminum precipitate may be heated to a temperature greater than 300°C, greater than 400°C, greater than 500°C, greater than 600°C, greater than 700°C, greater than 800°C, greater than 900°C, greater than 1000°C, greater than 1100°C, greater than 1200°C, greater than 1300°C, or greater than 1400°C.
[0137] In some embodiments, the precipitate can be heated to a temperature between 300°C and 1400°C, between 400 and 1400°C, between 500 and 1400°C, between 600 and 1400°C, between 700 and 1400°C, between 800 and 1400°C, between 900 and 1400°C, between 1000 and 1400°C, between 1100 and 1400°C, between 1200°C and 1400°C, or between 1300°C and 1400°C.
[0138] The calcining step may be carried out by heating the aluminum precipitate at a suitable temperature for a period of time sufficient to convert the aluminum precipitate to alumina, for example, the aluminum precipitate may be calcined for more than 15 seconds, more than 30 seconds, more than 1 minute, more than 5 minutes, more than 10 minutes, more than 15 minutes, more than 30 minutes, more than 45 minutes, more than 1 hour, more than 2 hours, more than 3 hours, more than 4 hours, more than 5 hours, or more than 6 hours.
[0139] In some embodiments, the precipitate can be calcined for between 15 seconds and 6 hours, between 30 seconds and 6 hours, between 1 minute and 6 hours, between 5 minutes and 6 hours, between 15 minutes and 6 hours, between 15 minutes and 6 hours, between 15 minutes and 6 hours, between 30 minutes and 6 hours, between 45 minutes and 6 hours, between 1 hour and 6 hours, between 2 hours and 6 hours, between 3 hours and 6 hours, between 4 hours and 6 hours, or between 5 hours and 6 hours.
[0140] As one skilled in the art will recognize, the temperature of calcination will determine the particular crystalline phase of Al2O3 that is formed, and thus, by moderate calcination temperatures, a variety of high purity aluminas with different crystalline structures can be produced.
[0141] In one particular embodiment, the dried precipitate may be calcined in two stages, the first to eliminate water from the crystal structure of the precipitate and the second to produce the desired crystal morphology of Al2O3.
[0142] A process for producing high purity alumina, according to one embodiment, will now be described with reference to the flowsheet shown in FIG.
[0143] Solid aluminum sulfate (1) is fed to a tank (3) with water (2) where it is mixed to provide an aqueous solution / slurry of aluminum sulfate. Recycled water (4) may also be used. The slurry (5) is pumped to a filter (6) where insoluble materials (7) are removed and discarded. The aluminum-containing solution (8) is fed to the loading stage (9) of the solvent extraction along with aqueous ammonia (10) to maintain pH. The aqueous solution is mixed with a liquid organic phase (11) containing D2EHPA. The aluminum is transferred to the organic phase (13) while the aluminum-reduced aqueous solution can be recycled (4) or discarded (12), for example by crystallization of ammonium sulfate.
[0144] The loaded organic phase (13) proceeds to stripping (14) where it is mixed with hydrochloric acid solution (15). The acid drives aluminum out of the organic phase, regenerating D2EHPA (11), which is returned to the loading stage (9). The aluminum solution (16) is fed to a precipitator (17) together with ammonia (18), which raises the pH and precipitates aluminum hydroxide. The resulting slurry (19) is fed to a filter (20), which separates the solution (21) from the precipitate (22). The solution (21) may be treated to separate and recover the HCl and NH3, or may be crystallized to ammonium chloride.
[0145] The precipitate (22) is fed to a calciner (23) where it is heated at 1250° C. for 4 hours to drive off water and convert the precipitate to HPA (24).
[0146] A process for producing high purity aluminum nitrate according to another embodiment will now be described with reference to the flowsheet shown in FIG.
[0147] Solid aluminum sulfate (1) is fed to a tank (3) with water (2) where the aluminum sulfate mixes and dissolves to produce an aqueous solution / slurry of aluminum salts. Recycled water (4) may also be used. The slurry (5) is pumped to a filter (6) where any insoluble material (7) is removed and discarded. The aluminum-containing solution (8) is fed to the loading stage (9) of the solvent extraction along with ammonia (10) to maintain pH. The aqueous solution is mixed with a liquid organic phase (11) containing D2EHPA. The aluminum is transferred to the organic phase (13) while the aluminum-reduced aqueous solution can be recycled (4) or discarded (12), for example by crystallization of ammonium sulfate.
[0148] The loaded organic phase (13) proceeds to stripping (14) where it is mixed with a nitric acid solution (15). The acid drives aluminium out of the organic phase, regenerating the D2EHPA (11), which is returned to the loading stage (9). The aluminium solution (16) is fed to an evaporator (17) where water is removed and aluminium nitrate crystals are produced. The resulting slurry (19) is fed to a filter (20) which separates the solution (18) from the product crystals (21). The solution (18) may be recycled back to the evaporation stage (17). EXAMPLES
[0149] The following examples are to be understood as merely illustrative, and therefore should not be construed as limiting the embodiments of the present disclosure in any way.
[0150] A clay sample was analyzed using X-ray diffraction and found to contain 30% quartz, 27% muscovite, 35% kaolinite and other clays.
[0151] To make the kaolinite suitable for leaching, it was necessary to convert the kaolin to metakaolin by calcination at 650°C for 4 hours. A mass loss of 4.5% was observed. Assays of the main elements present in the heads and calcined products are listed in Table 1.
[0152] JPEG0007591172000001.jpg75170
[0153] A solution of 32% HCl was heated to 80° C. and sufficient calcinate was added to give a slurry density of 40% solids (w / w). The extraction rates of major elements are shown in Figure 3. The reaction appears to be essentially complete within the first 60 minutes, and by 120 minutes there is little further change in concentration.
[0154] Table 3 shows the solution concentrations after 120 minutes.
[0155] JPEG0007591172000002.jpg75170
[0156] The slurry from the leaching test was filtered and the liquid was transported onwards to a series of solvent extraction (SX) separation stages.
[0157] The liquid from the HCl elution was contacted with 10% by volume Alamine 336 dissolved in kerosene. The aqueous and organic phases were mixed and then separated. The organic phase was drained and then contacted with deionized water in a 1:1 ratio to strip some of the metal impurities from the organic phase. The organic phase was then remixed with the aqueous phase followed by separation and stripping with deionized water as previously described, and this process was repeated a total of 10 times.
[0158] The extraction rates of metal impurities from the aqueous solution by the organic phase are shown in the table. Most of the Fe impurity is removed, while very little Al is lost. Several other metal impurities, Ba, Mn, S and Si, are also extracted. Water stripping of the supported organics removed all elements very efficiently.
[0159] JPEG0007591172000003.jpg32170
[0160] The aqueous solution separated from the original load (raffinate) has the assay shown in the table. This solution proceeds to Al-SX for aluminum enrichment and purification prior to precipitation.
[0161] JPEG0007591172000004.jpg100170
[0162] The raffinate was mixed with an organic solution of 20% by volume D2EHPA + 10% by volume TBP to extract aluminum. Table 6 shows the solution concentrations of the feed solution, the raffinate after Al extraction, and the solution after contacting the loaded organics with sulfuric acid.
[0163] Approximately 54% of the Al was extracted in a single extraction step. Without wishing to be bound by theory, it is believed that this represents the maximum possible loading of DEHPA, and that further extraction steps using fresh DEHPA would increase this to over 90%. There is no analytical data on the Al-SX raffinate, so no comments can be made regarding the extraction of other elements. The sulfuric acid used for stripping was 200 g / L and worked as expected by stripping the majority of the metals loaded on the D2EHPA.
[0164] JPEG0007591172000005.jpg108170
[0165] The data for Fe suggests that iron was more readily concentrated than Al. Fe is known to be more strongly extracted than Al using D2EHPA, and therefore Fe is loaded onto D2EHPA prior to Al, resulting in a greater proportion of Fe being extracted from the aqueous feed. Most importantly, the levels of Ca, K, Mg, Na, P, Ti and V are all significantly reduced in the strip solution.
[0166] The use of 200 g / L H2SO4 as the strip solution was to ensure complete stripping of the D2EHPA. Without wishing to be bound by theory, it is quite possible that more careful control of the pH of the strip solution could selectively strip Al from the D2EHPA while leaving Fe (and possibly other elements). Scrubbing of the loaded organics with a solution with higher Al concentration is also expected to further reduce impurity levels.
[0167] The strip solution that underwent Al SX was neutralized to a final pH of >6 using NaOH to precipitate Al. The feed and filtrate concentrations are shown in the table along with the percentage of elements precipitated. As can be seen, Al was fully precipitated while other elements were partially or not precipitated. The elements of interest are those with high starting concentrations (i.e., >1 ppm). The increase in Na and K in the filtrate was due to NaOH and the impurity K in NaOH. As can be seen, precipitation was quite effective for many elements other than Al, but only in small amounts since these elements are present at low levels. The amount of Na precipitated is unclear due to the use of NaOH to raise the pH. The use of ammonia to neutralize the solution eliminates the addition of Na or K to the solution.
[0168] JPEG0007591172000006.jpg101170
[0169] The aluminum precipitate was dried and calcined at 1200° C. for 4 hours to convert the precipitate to HPA, which was then partially washed in ultrapure water to remove any soluble surface ions.
[0170] The table shows the major impurities measured in the untreated and washed HPA. Any elements analyzed below the detection limit were accepted as being at the detection limit. This is especially important for S, which has a very high detection limit of 10 ppm, in fact the actual level may be somewhat lower. The major impurity elements were Si and Fe.
[0171] Ultrapure water was used to wash the HPA to remove any remaining soluble ions, and the data indicates that this step is critical to achieve the required purity of >99.99%. It should be noted that no loss of Al occurred during the washing step.
[0172] JPEG0007591172000007.jpg87170
[0173] The water used to wash the HPA may be replaced by an acid solution, which is expected to result in a higher removal rate of impurities without any damage to the HPA.
[0174] It will be understood by those skilled in the art that numerous variations and / or modifications may be made to the above-described embodiments without departing from the overall broad scope of the present disclosure, and the present embodiments are therefore to be considered in all respects as illustrative and not restrictive.
Claims
1. 1. A method for producing high purity alumina (HPA) from an aluminum-containing material, comprising: providing an aluminum-containing solution of the aluminum-containing material; selectively extracting aluminum from the aluminum-containing solution by liquid-liquid or liquid-solid extraction to obtain an aluminum-enriched organic liquid or an aluminum-enriched ion exchange resin; scrubbing the aluminum-enriched organic liquid or aluminum-enriched ion exchange resin with an aqueous solution to remove metal impurities therefrom, thereby producing a reduced-metal-impurity aluminum-enriched organic liquid or a reduced-metal-impurity aluminum-enriched ion exchange resin; stripping aluminum from the metal impurities-reduced, aluminum-rich organic liquid or the metal impurities-reduced, aluminum-rich ion exchange resin by contacting the liquid or resin with an acidic aqueous solution to produce an aluminum-rich aqueous solution; precipitating and separating an aluminum precipitate from said aluminum-rich aqueous solution; calcining the separated aluminum precipitate to produce HPA; A method comprising:
2. 1. A method for producing high purity aluminum salts from an aluminum-containing material, comprising the steps of: providing an aluminum-containing solution of the aluminum-containing material; selectively extracting aluminum from the aluminum-containing solution by liquid-liquid or liquid-solid extraction to obtain an aluminum-enriched organic liquid or an aluminum-enriched ion exchange resin; scrubbing the aluminum-enriched organic liquid or aluminum-loaded ion exchange resin with an aqueous solution to remove metal impurities therefrom, thereby producing a reduced-metal-impurity aluminum-enriched organic liquid or a reduced-metal-impurity aluminum-enriched ion exchange resin; stripping aluminum from the metal impurities-reduced, aluminum-rich organic liquid or the metal impurities-reduced, aluminum-rich ion exchange resin by contacting said liquid or resin with an acidic aqueous solution to produce an aluminum-rich aqueous solution; crystallizing and isolating high purity aluminum salts from the aluminum-rich aqueous solution; A method comprising:
3. 3. The method of claim 1 or 2, wherein the step of providing an aluminium-containing solution of the aluminium-containing material comprises dissolving the aluminium-containing material with an acid and separating the resulting aluminium-containing solution from any remaining insoluble material.
4. 3. The method according to claim 1 or 2, wherein the step of preparing an aluminium-containing solution of the aluminium-containing material may comprise dissolving the aluminium-containing material in water and separating the resulting aluminium-containing solution from any remaining insoluble material.
5. 3. The method of claim 1 or 2, wherein the step of selectively extracting aluminum from the aluminum-containing solution by liquid-liquid extraction comprises reacting the aluminum-containing solution with an extractant having selectivity for aluminum (the "aluminum extractant").
6. 6. The method of claim 5, wherein the aluminum extractant comprises one or more organophosphorus compounds selected from the group comprising organic derivatives of phosphoric acid, organic derivatives of phosphonic acid, organic derivatives of phosphinic acid or organic derivatives of dithiophosphinic acid, optionally in combination with a carboxylic acid, a ketoxime or an aldoxime compound.
7. 6. The method of claim 5, wherein the extractant is present in an organic liquid phase that is immiscible with the aluminum-containing solution, whereby the extractant reacts with the aluminum-containing solution to transfer aluminum from the aluminum-containing solution to the organic liquid phase to produce the aluminum-enriched organic liquid.
8. 3. The method of claim 1 or 2, wherein the step of selectively extracting aluminum from the aluminum-containing solution by liquid-solid extraction comprises contacting the aluminum-containing solution with an ion exchange resin having selectivity for aluminum compared to monovalent or divalent cations.
9. The method of claim 8 , wherein the ion exchange resin comprises a strong acid cation exchange resin or a weak acid cation exchange resin.
10. 3. The method of claim 1 or 2, wherein the step of scrubbing the aluminum-rich organic liquid comprises contacting the aluminum-rich organic liquid with an aqueous scrubbing solution to transfer trace metal impurities to the aqueous scrubbing solution, thereby producing an impurity-reduced aluminum-rich organic liquid phase and an impurity-rich aqueous phase.
11. The method of claim 10, wherein the aqueous scrubbing solution comprises a dilute acid or an aqueous solution of aluminum that is substantially free of metal impurities.
12. 11. The method of claim 10, wherein the aqueous scrubbing solution comprises a bleed stream of the aluminum-rich aqueous solution obtained by stripping an aluminum-bearing organic liquid.
13. 3. The method of claim 1 or 2, wherein the step of stripping the metal impurities-reduced, aluminum-enriched organic liquid or the metal impurities-reduced, aluminum-enriched ion exchange resin comprises contacting the liquid or the resin with an acidic aqueous solution having a pH of 3 or less.
14. 3. The method of claim 2, wherein the step of crystallizing a high purity aluminum salt from the aluminum-rich solution comprises evaporating sufficient solvent from the aluminum-rich solution to exceed the solubility product of the high purity aluminum salt.
15. 2. The method of claim 1, wherein the step of precipitating an aluminum precipitate from the aluminum-rich solution comprises increasing the pH of the solution to a range of 4 to 11.
16. Increasing the pH of the solution may be achieved by the addition of aqueous ammonia, NH 4 16. The method of claim 15, comprising adding OH to the solution.
17. The aluminum precipitate is tetrahydroaluminate [Al(OH) 4 ] - compound, aluminum oxyhydroxide, AlOOH compound or aluminum hydroxide Al(OH) 3 The method of claim 1 comprising the compound.
18. The method of claim 1 , wherein the precipitating step is carried out at elevated temperature and, optionally, elevated pressure.
19. 20. The method of claim 18, wherein the precipitating step is maintained at the elevated temperature, and optionally elevated pressure, for between 15 minutes and 48 hours.
20. 2. The method of claim 1, wherein the step of calcining the aluminum precipitate is carried out at a temperature between 300°C and 1400°C.
21. The calcination step is performed in a first stage at a first temperature for a period of time sufficient to drive off water of crystallization from the aluminum precipitate, and in a second stage at a temperature higher than the first temperature to convert the aluminum precipitate into corundum (α-Al 2 O 3 ), for a period sufficient to convert the β-alumina or other alumina polymorphs.
22. 2. The method of claim 1, further comprising separating one or more metal impurities, in particular iron, from the aluminium-containing solution prior to selectively extracting aluminium from the aluminium-containing solution.
23. 23. The method of claim 22, wherein the further step of separating iron impurities from the aluminum-containing solution comprises selectively extracting the iron impurities by liquid-liquid extraction or liquid-solid extraction to obtain an iron-reduced aluminum-containing solution.
24. 24. The method of claim 23, wherein the step of selectively extracting iron impurities from the aluminum-containing solution by liquid-liquid extraction comprises reacting the aluminum-containing solution with an iron extractant that is selective for iron.
25. 25. The method of claim 24, wherein the iron extractant comprises a synergistic mixture of di(2-ethylhexyl) hydrogen phosphate and tributyl phosphate, or a primary amine in its free base form.
26. 24. The method of claim 23, wherein the step of selectively extracting iron impurities from the aluminum-containing solution by liquid-solid extraction comprises contacting the aluminum-containing solution with an ion exchange resin having selectivity for iron impurities.