Manufacturing method of hot-rolled steel sheet, method for predicting temperature history of hot-rolled steel sheet, and method for predicting hardened portion of hot-rolled steel sheet

The method predicts the temperature history and phase transformation rates of hot-rolled steel sheet coil ends to prevent cracks and breakage during cold rolling, enhancing production efficiency and reducing restoration costs.

JP7591447B2Active Publication Date: 2024-11-28KOBE STEEL LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021049930
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-03-25
Filing Date
2021-03-24
Publication Date
2024-11-28
Estimated Expiration
2041-03-24

AI Technical Summary

Technical Problem

Hot-rolled steel sheets often break during cold rolling due to cracks at the edges caused by uneven cooling rates at convex portions of the coil ends, leading to increased restoration costs and equipment failure.

Method used

A method to predict the temperature history of the coil end face unevenness by measuring the surface temperature, calculating the temperature history, and using a displacement meter to derive the size of the unevenness, allowing for accurate prediction of phase transformation rates and potential material breakage.

Benefits of technology

Enables early detection of potential material fractures, reducing the risk of breakage and equipment failure by optimizing manufacturing conditions based on the predicted temperature history and phase transformation rates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007591447000011
    Figure 0007591447000011
  • Figure 0007591447000012
    Figure 0007591447000012
  • Figure 0007591447000013
    Figure 0007591447000013
Patent Text Reader

Abstract

To provide a method for manufacturing a hot-rolled steel sheet which can predict a temperature history of unevenness on an end face of a coil.SOLUTION: A method for manufacturing a hot-rolled steel sheet according to one aspect of the present invention includes steps of: measuring a surface temperature of a strip-like hot-rolled steel material; calculating a temperature history in a cooled state after winding when it is supposed that the strip-like steel material is wound in a coil shape with no unevenness on an end face on the basis of the surface temperature measured in the measurement step; actually winding the strip-like steel material after the measurement step in a coil shape; scanning the end face of the coil wound in the winding step with a displacement gauge, and deriving a size of the unevenness on the end face in a radius of the coil; and predicting a temperature history of the unevenness in the cooled state using the temperature history calculated in the calculation step and the size of the unevenness derived in the derivation step.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for manufacturing a hot-rolled steel sheet, a method for predicting the temperature history of a hot-rolled steel sheet, and a method for predicting a hardened portion of a hot-rolled steel sheet. [Background technology]

[0002] Hot-rolled steel sheets are manufactured by winding up hot-rolled steel strips into coils and cooling the coils to room temperature. The hot-rolled steel sheets are then re-spun into strips, pickled and cold-rolled to produce cold-rolled steel sheets. One problem in the manufacture of cold-rolled steel sheets is breakage of the steel sheets during threading. If breakage occurs in the steel sheets, the threading line must be stopped to perform recovery work, which increases the cost of recovery and reduces production efficiency. Furthermore, breakage of the steel sheets can also cause equipment failures. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2014-593 A [Patent Document 2] JP 2010-112958 A Summary of the Invention [Problem to be solved by the invention]

[0004] One of the causes of breakage during cold rolling of steel with high hardenability is cracks at the ends of the steel. If a crack occurs at the end of a steel material during cold rolling, stress is concentrated at the cracked part during threading, causing the crack to grow and leading to breakage of the steel material.

[0005] One of the causes of these cracks is a faulty winding shape of the hot-rolled coil. In other words, if there is a fault in winding the coil after hot rolling, the unevenness of the end surface of the coil will become large. If there are large protrusions on the coil end surface, the protrusions will function as fins and the cooling rate of the protrusions will increase when the coil is cooled. If the cooling rate of the protrusions increases, hard phases such as bainite and martensite will tend to be mixed in the protrusions. As a result, voids will be generated during cold rolling of the steel material, and as these voids grow, they will easily cause cracks at the ends.

[0006] From this perspective, the inventors discovered that by predicting the temperature history of the unevenness (particularly the convex parts) on the end surface of the coil, it is possible to detect in advance the possibility of the steel material breaking in the subsequent processes.

[0007] Patent Document 1 describes a method of predicting temperature unevenness of a hot-rolled steel sheet on a run-out table (ROT) and controlling the manufacturing conditions of the rolled steel sheet before it is wound on a coiler so as to reduce the predicted temperature unevenness.

[0008] Patent Document 2 also describes a technique for scanning a distance meter over the coil diameter on the end face of a metal plate coil, measuring the distance between the distance meter and the coil end face, and calculating the telescope amount of the coil end face, in which the measured value of the coil end part is identified as a tongue-shaped part or a telescope-shaped part. Patent Document 2 describes a technique for determining that a coil in which the difference in the measured distance between the innermost metal plates at both ends of the coil inner diameter or the difference in the measured distance between the outermost metal plates at both ends of the coil outer diameter exceeds a threshold value has measured the tongue-shaped part of the coil end of the metal plate, and excluding the innermost turn and / or outermost turn distance data in which the tongue-shaped part is measured, to calculate the telescope amount of the coil.

[0009] However, Patent Documents 1 and 2 do not consider the relationship between unevenness on the coil end surface and cracks in the coil end.

[0010] The present invention has been made based on the above-mentioned circumstances, and aims to provide a manufacturing method for a hot-rolled steel sheet capable of predicting the temperature history of unevenness on the end surface of a coil, and a method for predicting the temperature history of a hot-rolled steel sheet. Another aim of the present invention is to provide a method for predicting the hardened part of a hot-rolled steel sheet capable of predicting the presence or absence of fracture of a steel material in a subsequent process based on the temperature history of unevenness on the end surface of a coil. [Means for solving the problem]

[0011] A method for manufacturing hot-rolled steel sheet according to one embodiment of the present invention includes a measurement step for measuring the surface temperature of hot-rolled strip steel, a first calculation step for calculating the temperature history in a cooled state after winding, assuming that the strip steel is wound into a coil without any unevenness on the end surface, based on the surface temperature measured in the measurement step, a winding step for actually winding the strip steel into a coil after the measurement step, a derivation step for scanning the end surface of the coil wound in the winding step with a displacement meter and deriving the magnitude of unevenness on the end surface over the radius of the coil, and a first prediction step for predicting the temperature history of the unevenness in a cooled state using the temperature history calculated in the first calculation step and the magnitude of unevenness derived in the derivation step.

[0012] The method for manufacturing a hot-rolled steel sheet makes it possible to predict the temperature history of the unevenness of the end surface of the coil formed by winding the strip steel material while it is naturally cooling.

[0013] The manufacturing method of the hot-rolled steel sheet may further include a second calculation step of calculating a phase transformation rate using the temperature history predicted in the first prediction step, and a second prediction step of predicting a hardened portion of the strip steel material using the phase transformation rate calculated in the second calculation step. By including the second calculation step and the second prediction step, the manufacturing method of the hot-rolled steel sheet can predict the presence or absence of fracture of the steel material in a subsequent process.

[0014] In the deriving step, the magnitude of the unevenness may be calculated based on the median value of the measurements by the displacement meter. In this way, by calculating the magnitude of the unevenness based on the median value of the measurements by the displacement meter in the deriving step, the temperature history of the unevenness of the end surface of the coil in a cooled state can be easily and accurately predicted.

[0015] In the deriving step, the size of the unevenness may be calculated using a two-dimensional coordinate system defined by the direction in which the unevenness protrudes and the scanning direction of the displacement gauge. In this way, by calculating the size of the unevenness in the deriving step using a two-dimensional coordinate system defined by the direction in which the unevenness protrudes and the scanning direction of the displacement gauge, the temperature history of the unevenness of the end surface of the coil in a cooled state can be easily and accurately predicted.

[0016] A method for predicting the temperature history of hot-rolled steel sheet according to another embodiment of the present invention includes a measurement step of measuring the surface temperature of hot-rolled strip steel, a first calculation step of calculating the temperature history in a cooled state after winding, assuming that the strip steel is wound into a coil without any unevenness on the end surface, based on the surface temperature measured in the measurement step, a winding step of actually winding the strip steel into a coil after the measurement step, a derivation step of scanning the end surface of the coil wound in the winding step with a displacement meter and deriving the magnitude of unevenness on the end surface over the radius of the coil, and a first prediction step of predicting the temperature history of the unevenness in a cooled state using the temperature history calculated in the first calculation step and the magnitude of unevenness derived in the derivation step.

[0017] The method for predicting the temperature history of a hot-rolled steel sheet can predict the temperature history of the unevenness of the end surface of the coil formed by winding the strip steel material while it is cooled.

[0018] A method for predicting a hardened portion of a hot-rolled steel sheet according to another aspect of the present invention includes a measurement step of measuring the surface temperature of a hot-rolled strip steel material, a first calculation step of calculating a temperature history in a cooling state after winding, assuming that the strip steel material is wound into a coil shape without unevenness on the end surface, based on the surface temperature measured in the measurement step, a winding step of actually winding the strip steel material after the measurement step into a coil shape, a derivation step of scanning the end surface of the coil wound in the winding step with a displacement meter and deriving the magnitude of unevenness on the end surface over the radius of the coil, a first prediction step of predicting the temperature history of the unevenness in a cooling state using the temperature history calculated in the first calculation step and the magnitude of the unevenness derived in the derivation step, a second calculation step of calculating a phase transformation rate using the temperature history predicted in the first prediction step, and a second prediction step of predicting a hardened portion of the strip steel material using the phase transformation rate calculated in the second calculation step.

[0019] The method for predicting hardened portions of a hot-rolled steel sheet can predict whether or not the steel material will break in a subsequent process based on the temperature history of the unevenness of the end surface of the coil. Effect of the Invention

[0020] As described above, the manufacturing method of a hot-rolled steel sheet according to one aspect of the present invention and the method for predicting the temperature history of a hot-rolled steel sheet according to another aspect of the present invention can predict the temperature history of the unevenness of the end surface of a coil. Also, the method for predicting the hardened portion of a hot-rolled steel sheet according to another aspect of the present invention can predict the presence or absence of fracture of the steel material in a subsequent process based on the temperature history of the unevenness of the end surface of a coil. [Brief description of the drawings]

[0021] [Figure 1] FIG. 1 is a flow diagram showing a method for producing a hot-rolled steel sheet according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic diagram showing a hot-rolled steel sheet manufacturing facility used in the method for manufacturing a hot-rolled steel sheet shown in FIG. [Diagram 3] FIG. 3 is an explanatory diagram of a procedure for calculating the temperature history of the imaginary coil in the first calculation step of the manufacturing method of the hot-rolled steel sheet in FIG. [Figure 4] FIG. 4 is a schematic diagram showing the scanning position of the end surface of the coil by the displacement meter in the derivation step of the manufacturing method of the hot-rolled steel sheet in FIG. [Diagram 5] FIG. 5 is an explanatory diagram of a procedure for deriving the magnitude of unevenness in the deriving step of the manufacturing method of the hot-rolled steel sheet in FIG. [Figure 6] FIG. 6 is a flow diagram showing a method for producing a hot-rolled steel sheet according to a different embodiment from the method for producing a hot-rolled steel sheet shown in FIG. [Figure 7] FIG. 7 is a graph showing the temperature history of the upper end surface of the imaginary coil obtained in the first calculation step No. 1 in a cooled state, with the temperature immediately after winding as the reference point. [Figure 8] FIG. 8 is a graph showing the measurement results of the shape of the unevenness on the end surface of the coil by the displacement meter in the derivation process No. 1 and the derivation results of the magnitude of the unevenness on the end surface of the coil by the derivation unit. [Figure 9] FIG. 9 is a graph showing the temperature history of the end surface of the coil in a cooled state, based on the temperature immediately after winding, predicted in the first prediction step of No. 1, and the actual measured temperature of this end surface. [Figure 10] FIG. 10 is a graph showing the temperature history of the upper end surface in a naturally cooled state, calculated in the first calculation step of No. 2, with the temperature immediately after winding of the imaginary coil as the reference. [Figure 11] FIG. 11 is a graph showing the measurement results of the shape of the unevenness on the end surface of the coil by the displacement meter in the derivation process No. 2 and the derivation results of the magnitude of the unevenness on the end surface of the coil by the derivation unit. [Figure 12] FIG. 12 is a graph showing the temperature history of the end surface of the coil in a cooled state, based on the temperature immediately after winding, predicted in the first prediction step of No. 2, and the actual measured temperature of this end surface. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings.

[0023] [First embodiment] <Method of manufacturing hot-rolled steel sheets> The manufacturing method of hot-rolled steel sheet in FIG. 1 includes a step of measuring the surface temperature of hot-rolled strip steel (measurement step S1), a step of calculating the temperature history in a cooling state after winding, assuming that the strip steel is wound into a coil with no unevenness on the end surface, based on the surface temperature measured in the measurement step S1 (first calculation step S2), a step of actually winding the strip steel into a coil after the measurement step S1 (winding step S3), a step of scanning the end surface of the coil wound in the winding step S3 with a displacement meter and deriving the magnitude of unevenness on the end surface over the radius of the coil (deriving step S4), and a step of predicting the temperature history of the unevenness in a cooling state using the temperature history calculated in the first calculation step S2 and the magnitude of unevenness derived in the derivation step S4 (first prediction step S5). The measuring step S1, the first calculating step S2, the winding step S3, the deriving step S4, and the first predicting step S5 constitute a method for predicting the temperature history of a hot-rolled steel sheet according to one embodiment of the present invention. Note that the term "coil-shaped" refers to a spiral shape when viewed in the axial direction. The term "end face of the coil" refers to a surface of the coil that is perpendicular to the central axis. In other words, the term "end face of the coil" refers to a surface formed by an end of the strip steel material in the width direction.

[0024] According to this method for manufacturing hot-rolled steel sheet, by predicting the temperature history of the unevenness of the end surface of the coil, it is possible to detect in advance the possibility of the steel breaking when using this hot-rolled steel sheet to manufacture a cold-rolled sheet.

[0025] In describing the manufacturing method of the hot-rolled steel sheet, first, with reference to FIG. 2, a manufacturing facility 1 for the hot-rolled steel sheet (hereinafter, also simply referred to as "manufacturing facility 1") capable of carrying out the manufacturing method of the hot-rolled steel sheet will be described.

[0026] [Hot-rolled steel sheet manufacturing equipment] The manufacturing equipment 1 of FIG. 2 includes a hot rolling apparatus 2 that includes a plurality of pairs of rolling rolls 2a, a conveying section 2b that conveys the strip steel X hot-rolled by the rolling rolls 2a, and a winding machine 2c that winds up the strip steel X conveyed to the conveying section 2b into a coil, and is provided with a hot rolling line, a measuring device 3 that measures the surface temperature of the strip steel X being conveyed to the conveying section 2b, a calculating device 4 that calculates the temperature history of a coil (virtual coil) in a cooling state when it is assumed that the strip steel X is wound into a coil shape without unevenness on the end surface based on the surface temperature of the strip steel X measured by the measuring device 3, a derivation device 5 that constitutes a derivation line that derives the magnitude of unevenness on the end surface E of the coil X1 wound by the winding machine 2c over the radius of the coil X1, and a prediction device 6 that predicts the temperature history of the unevenness in a cooling state using the temperature history calculated by the calculating device 4 and the magnitude of unevenness derived by the derivation device 5. The manufacturing equipment 1 also includes a cooling device 7 that cools the coil X1 after passing through the lead-out line. The manufacturing equipment 1 may further include a cold rolling device that cold-rolls the coil X1 after being cooled by the cooling device 7, an annealing device that anneals the strip steel material after being cold-rolled by the cold rolling device, and the like.

[0027] The hot rolling mill 2 performs rough rolling and finish rolling on a thick steel plate heated in a heating furnace (not shown), and then transports the rolled strip steel X to a winding machine 2c by a transport section 2b, and winds it into a coil by the winding machine 2c. The transport section 2b has, for example, a plurality of transport rollers.

[0028] The measuring device 3 has a non-contact temperature sensor 3a such as a thermograph. The measuring device 3 measures the surface temperature of the strip steel material X after hot rolling and before it is wound by the winder 2c. The measuring device 3 measures the temperature of the entire surface area (total length and width) of the strip steel material X.

[0029] The calculation device 4 is composed of, for example, a computer. The calculation device 4 assumes that a coil (virtual coil) formed by winding, for example, a steel strip X, has a cylindrical end surface with no irregularities, and calculates the temperature history of this virtual coil in a cooling state using a two-dimensional model in a polar coordinate system.

[0030] The lead-out device 5 includes a conveyor 5a for transporting the coil X1 wound by the winding machine 2c, a displacement meter 5b for scanning the end face E of the coil X1 transported on the conveyor 5a and measuring the shape of the end face E, and a lead-out unit 5c for deriving the magnitude of the unevenness of the end face E of the coil X1 based on the shape measured by the displacement meter 5b. The displacement meter 5b measures the shape of the end face E of the coil X1 over the radius of the coil X1, and preferably over the diameter. For example, a laser displacement meter is used as the displacement meter 5b. The displacement meter 5b includes a laser irradiation unit that irradiates the end face E of the coil X1 with laser light, and a light receiving element that receives a part of the light reflected by the end face E. The displacement meter 5b reads the reflected light of the laser light irradiated from the laser irradiation unit to the end face E by the light receiving element. The displacement meter 5b is configured to be able to measure the shape of the end face E of the coil X1 by a triangulation method. The derivation unit 5c is constituted by, for example, a computer. The displacement meter 5b and the derivation unit 5c may be integrally constituted.

[0031] The prediction device 6 is composed of, for example, a computer. The prediction device 6 predicts the temperature history of the unevenness of the end surface E of the coil X1 when it is assumed that the coil X1 actually wound by the winding machine 2c is cooled by a cooling device 7 or the like.

[0032] The cooling device 7 cools the coil X1 after the shape of the end face E is measured by the measuring device 3. In the manufacturing equipment 1, the coil X1 is heated to about 500°C or higher after being wound by the winding machine 2c. The cooling device 7 air-cools the heated coil X1 to room temperature. Since the manufacturing equipment 1 cools the coil X1 wound by the winding machine 2c, if a large protrusion is present on the end face E of the coil X1, the cooling rate of the protrusion is likely to be faster than other parts.

[0033] [Strip steel] The strip steel X is formed by heating a slab and hot rolling it. The strip steel X has a composition of, for example, carbon, silicon, manganese, phosphorus, sulfur, chromium, nickel, molybdenum, and copper, with the balance being iron and unavoidable impurities. When cold rolling is applied to the strip steel X, the coiling temperature in the coiling step S3 can be set to be equal to or higher than Ms (martensitic transformation start temperature) of the strip steel X.

[0034] The upper limit of the carbon equivalent Ceq of the strip steel X, expressed by the following formula (1), is preferably 0.75%, more preferably 0.70%. If the carbon equivalent Ceq of the strip steel X exceeds the above upper limit, the possibility of the martensite phase being generated increases when the cooling rate during natural cooling is high. On the other hand, the lower limit of the carbon equivalent Ceq is not particularly limited, but can be, for example, 0.55%. If the carbon equivalent Ceq does not meet the above lower limit, the transformation is generally completed by the time of the coiling process S3, so that the martensite phase is unlikely to be generated, and the risk of edge cracking occurring in the coil X1 in the subsequent process is low. Therefore, the manufacturing method of the hot-rolled steel sheet is suitably used when the carbon equivalent Ceq of the strip steel X is equal to or greater than the above lower limit. Ceq[%]=[C]+[Si] / 24+[Mn] / 6+[Ni] / 40+[Cr] / 5+[Mo] / 4+[V] / 14...(1) Here, [C], [Si], [Mn], [Ni], [Cr], [Mo] and [V] indicate the contents (mass%) of C, Si, Mn, Ni, Cr, Mo and V, respectively.

[0035] (Measurement process) The measuring step S1 is performed by a measuring device 3. In the measuring step S1, the surface temperature of the strip steel material X after hot rolling and before being wound by the winder 2c is measured over the entire surface area (full length and full width) of the strip steel material X.

[0036] (1st calculation step) The first calculation step S2 is performed by a calculation device 4. In the first calculation step S2, for example, a coil (virtual coil) formed by winding the strip steel X and having no irregularities on its end surface is assumed to be cylindrical, and the temperature history of this virtual coil in a cooling state is calculated by a two-dimensional model in a polar coordinate system. The first calculation step S2 may be performed before or after the winding step S3. The first calculation step S2 may also be performed after the derivation step S4.

[0037] An example of a calculation procedure of the temperature history of the virtual coil X2 in the naturally cooled state by the first calculation step S2 will be described with reference to Fig. 3. In the first calculation step S2, the coordinate of the intersection between a virtual plane including one end face (upper end face in Fig. 3) of the virtual coil X2 and the central axis of the virtual coil X2 is set as the origin O (0, 0), the coordinate in the central axis direction based on the origin O is z [m], and the coordinate in the radial direction based on the origin O is r [m], and the temperature history of the virtual coil X2 in the naturally cooled state is calculated using a two-dimensional model of a polar coordinate system. In the first calculation step S2, a plurality of calculation points are provided in each of the central axis direction and the radial direction of the virtual coil X2, and the temperature history in the naturally cooled state is calculated for each calculation point. Specifically, in the first calculation step S2, the following formula (2) is used for calculation points inside the imaginary coil X2 (calculation points of the parts not exposed to the outside air), and the following formula (3) is used for calculation points of the parts exposed to the outside air. The temperature after time t at the calculation points of the imaginary coil X2, which is based on the time immediately after winding, is defined as Φ [°C], and the temperature history of the imaginary coil X2 in the cooled state is calculated.

[0038]

number

[0039]

number

[0040] In the above formulas (2) and (3), H is enthalpy [kcal / kg], ρ is density [kg / m 3 ], λ r: Radial thermal conductivity [kcal / m / hr / ℃], λ z : Axial thermal conductivity [kcal / m / hr / ℃], ε: Emissivity [-], σ: Stefan-Boltzmann constant [kcal / m 2 / hr / ℃ 4 ], F 12 : View factor [-], α: Natural convection heat transfer coefficient [kcal / hr / m 2 / ℃], V: Volume of the part of the steel strip corresponding to the calculation point [m 3 ], A: Surface area [m 2 In the above formula (3), q is a boundary condition. This boundary condition is given by the following formula (4) for the inner peripheral surface of the imaginary coil X2, and by the following formula (5) for the end and outer peripheral surfaces of the imaginary coil X2. In the following formulas (4) and (5), T: surface temperature [°C] measured in the measurement step S1 of the portion corresponding to the calculation point, T f : Ambient temperature when cooled [℃].

[0041]

number

[0042]

number

[0043] (winding process) In the winding step S3, the strip steel X after the surface temperature is measured in the measurement step S1 is wound into a coil shape at a high temperature by the winding machine 2c. The winding temperature in the winding step S3 is preferably equal to or higher than the Ms temperature of the strip steel X from the viewpoint of preventing the formation of martensite phase. The lower limit of the winding temperature is preferably 400°C, more preferably 500°C, and even more preferably 560°C. On the other hand, the upper limit of the winding temperature is preferably 700°C, and more preferably 670°C. If the winding temperature does not reach the lower limit, the strength of the strip steel X may become too large, which may increase the load on the equipment in the subsequent process such as the cold rolling process. Conversely, if the winding temperature exceeds the upper limit, the scale thickness on the surface of the strip steel X may become large. The "winding temperature" refers to the surface temperature of the strip steel X immediately before winding.

[0044] (Derivation process) The lead-out process S4 is performed by the lead-out device 5. As shown in FIG. 2 and FIG. 4, in the lead-out process S4, the end face E of the coil X1 transported on the conveyor 5a is scanned by the displacement meter 5b, and the shape of the unevenness of the end face E is measured over the radius of the coil X1, preferably over the diameter. Furthermore, in the lead-out process S4, the lead-out unit 5c obtains the magnitude of the unevenness of the end face E using a two-dimensional coordinate system defined by the protruding direction of the unevenness (the central axis direction of the coil X1) and the scanning direction by the displacement meter 5b (the radial direction of the coil X1). In the manufacturing method of the hot-rolled steel sheet, by obtaining the magnitude of the unevenness of the end face E using the above-mentioned two-dimensional coordinate system, the temperature history of the unevenness of the end face E of the coil X1 in the cooling state can be easily and accurately predicted by the first prediction process S5 described later.

[0045] In the derivation step S4, it is preferable to obtain the magnitude of unevenness of the end face E based on the median value of the measurement value by the displacement meter 5b. Specifically, in the derivation step S4, it is preferable to continuously measure the end face E of the coil X1 over the radius by the displacement meter 5b, and then obtain the magnitude of unevenness of the end face E based on the median value of the measurement value by the displacement meter 5b by the derivation unit 5c. In the manufacturing method of the hot-rolled steel sheet, by obtaining the magnitude of unevenness of the end face E based on the above-mentioned median value, it is possible to appropriately measure the magnitude of unevenness of the entire coil X1 even in cases where a large protruding portion (telescope) due to winding slippage is formed at the end of the outer circumferential side and / or inner circumferential side of the coil X1. As a result, the first prediction step S5 makes it easy to easily and accurately predict the temperature history of the unevenness of the end face E of the coil X1 in the cooling state.

[0046] With reference to FIG. 4 and FIG. 5, an example of a procedure for deriving the magnitude of unevenness of the end face E of the coil X1 in the deriving step S4 will be described. First, in the deriving step S4, the end face E of the coil X1 conveyed on the conveyor 5a is scanned by the displacement meter 5b, and the shape of the unevenness of the end face E is measured over the radius of the coil X1. Next, a reference plane R of the end face E is set based on the median value of the measurement values ​​by the displacement meter 5b. Next, the magnitude of unevenness of the end face E is obtained using a two-dimensional model of a polar coordinate system in which the coordinate of the intersection between the central axis Z of the coil X1 and the reference plane R is set as the origin O (0, 0), the coordinate in the central axis direction based on the origin O is z [m], and the coordinate in the radial direction based on the origin O is r [m]. Specifically, the coil X1 is divided into a plurality of regions in the radial direction, the magnitude of unevenness is averaged for each region, and this average value is inserted into the two-dimensional coordinate system to derive the magnitude of unevenness of this region. In this case, it is also possible that the length of each region in the radial direction of the coil X1 is not the same. For example, the length of a pair of regions located at both ends in the radial direction may be set to be smaller than the other regions so that it is easier to reflect the unevenness caused by the telescope. It is also possible to set a certain threshold and treat the amount of protrusion below this threshold as not corresponding to unevenness.

[0047] (First prediction step) The first prediction step S5 is performed by the prediction device 6. In the first prediction step S5, the temperature history of the unevenness of the end face E of the coil X1 in a naturally cooled state is predicted, with the time immediately after winding as a reference. In the first prediction step S5, the temperature history of the unevenness of the end face E in a naturally cooled state is predicted using the above-mentioned formulas (2) to (5). At this time, for the reference plane R, the boundary condition of the above-mentioned formula (3) is given by the above-mentioned formula (5).

[0048] <Advantages> The manufacturing method of the hot-rolled steel sheet can predict the temperature history of the unevenness of the end surface E of the coil X1 formed by winding the strip steel X in a cooling state. Therefore, the manufacturing method of the hot-rolled steel sheet can detect the possibility of steel fracture in advance when manufacturing a cold-rolled sheet using the strip steel X.

[0049] The method for predicting the temperature history of a hot-rolled steel sheet can predict the temperature history of the unevenness of the end surface E of the coil X1 formed by winding the strip steel X in a cooling state. Therefore, the method for predicting the temperature history of a hot-rolled steel sheet can detect in advance the possibility of steel material fracture when a cold-rolled sheet is manufactured using the strip steel X.

[0050] [Second embodiment] <Method of manufacturing hot-rolled steel sheets> The method for manufacturing the hot-rolled steel sheet in FIG. 6 includes a step of measuring the surface temperature of a hot-rolled steel strip (measurement step S11), a step of calculating a temperature history in a cooling state after winding, assuming that the steel strip is wound into a coil without unevenness on its end surface, based on the surface temperature measured in the measurement step S11 (first calculation step S12), a step of actually winding the steel strip after the measurement step S11 into a coil (winding step S13), and a step of scanning the end surface of the coil wound in the winding step S13 with a displacement meter to calculate the magnitude of unevenness on the end surface. The method includes a step of deriving the temperature history over the radius of the coil (deriving step S14), a step of predicting the temperature history of the unevenness in a cooling state using the temperature history calculated in the first calculation step S12 and the size of the unevenness derived in the derivation step S14 (first prediction step S15), a step of calculating a phase transformation rate (ferrite-pearlite transformation rate) using the temperature history predicted in the first prediction step S15 (second calculation step S16), and a step of predicting the hardened portion of the strip steel material using the phase transformation rate calculated in the second calculation step S16 (second prediction step S17). The measurement step S11, the first calculation step S12, the coiling step S13, the derivation step S14, the first prediction step S15, the second calculation step S16, and the second prediction step S17 constitute a method of predicting the hardened portion of a hot-rolled steel sheet according to one aspect of the present invention. The measurement step S11, the first calculation step S12, the winding step S13, and the leading out step S14 can be performed in the same manner as the measurement step S1, the first calculation step S2, the winding step S3, and the leading out step S4 in Fig. 1, and therefore the description thereof will be omitted. Note that in the first calculation step S12, as in the first prediction step S15 described later, the temperature history may be calculated using the following formula (6) instead of the above formula (2) and the following formula (7) instead of the above formula (3).

[0051] (First prediction step) In the first prediction step S15, the transformation heat generation amount Q for each time calculated in the second calculation step S16 described later is calculated. t [kcal / m 3 / hr] is added to obtain the temperature history of the strip steel material. Specifically, in the first prediction step S15, the temperature history is predicted using the following formula (6) instead of the above formula (2) and using the following formula (7) instead of the above formula (3). The first prediction step S15 can be performed in the same manner as the first prediction step S5 in FIG. 1, except that the following formula (6) is used instead of the above formula (2) and the following formula (7) is used instead of the above formula (3).

[0052]

number

[0053]

number

[0054] (Second calculation process) The second calculation step S16 can be performed by, for example, a computer. In the second calculation step S16, the phase transformation rate is calculated from an isothermal transformation equation including the effect of the γ grain size. In addition, in the second calculation step S16, the transformation heat generation amount Q according to the calculated phase transformation rate is calculated. t Specifically, in the second calculation step S16, the phase transformation rate X[-] is calculated by the following formula (8) and the following formula (9), and the transformation heat generation amount Q at time t is calculated by the following formula (10). t [kcal / m 3 / hr] is calculated. t is used to predict the temperature history in the first prediction step S15 described above. In addition, this transformation heat generation amount Q t may be used to calculate the temperature history in the first calculation step S12 described above.

[0055]

number

[0056]

number

[0057]

number

[0058] In the above formulas (8) to (10), S is the nucleation area term, K is the temperature-dependent term, and Q total : Total transformation heat [kcal / m 3 / hr], T: temperature [°C] of the calculation point calculated in the first calculation step S12 or the first prediction step S15. In addition, a, b, c, m, and n in the above formulas (8) to (10) are constants adjusted for each type of steel. These constants can be determined by, for example, creating a TTT diagram using a hot rolled crop after rough rolling and adjusting the calculated values ​​so that they match the experimental values. However, the transformation rate is affected by the state of the pre-transformation structure, such as the austenite grain size, and therefore varies depending on the hot rolling conditions. Therefore, the value of c is adjusted for each hot rolling condition.

[0059] (Second prediction step) The second prediction step S17 can be performed by, for example, a computer. In the second prediction step S17, the phase transformation rate calculated in the second calculation step S16 is used to predict the hardened portion of the end surface of the coil wound in the winding step S13. In the second prediction step S17, for example, the relationship between the phase transformation rate and the hardness is obtained in advance, and the hardened portion is predicted from the calculated phase transformation rate. In the second prediction step S17, for example, a threshold value of the hardness at which the steel material may break in a subsequent step such as a cold rolling step may be set in advance, and the calculated phase transformation rate may be compared with this threshold value to predict the presence or absence of breakage in the steel material in the subsequent step. In addition, in the second prediction step S17, a threshold value of the phase transformation rate at which the steel material may break in a subsequent step such as a cold rolling step may be set in advance, and the calculated value may be compared with this threshold value to predict the presence or absence of breakage in the steel material.

[0060] <Advantages> The manufacturing method of the hot-rolled steel sheet can predict whether or not the steel will break in a later process by using the phase transformation ratio calculated in the second calculation step S16. According to the manufacturing method of the hot-rolled steel sheet, the risk of the steel breaking during threading can be reduced by previously removing the hardened portion that may cause the steel to break in a later process.

[0061] The method for predicting hardened portions in a hot-rolled steel sheet can predict the presence or absence of fracture of the steel material in a subsequent process by using the phase transformation rate calculated in the second calculation step S16.

[0062] [Other embodiments] The above-mentioned embodiment does not limit the configuration of the present invention. Therefore, the above-mentioned embodiment may omit, replace or add components of each part of the above-mentioned embodiment based on the description in this specification and common technical knowledge, and it should be understood that all of these are within the scope of the present invention.

[0063] For example, in the deriving step, it is also possible to determine the magnitude of unevenness of the end surface of the coil based on the average value, mode, etc. However, as described above, in the deriving step, from the viewpoint of being able to properly measure the magnitude of unevenness of the entire coil even when a large protruding portion such as a telescope is present, it is preferable to determine the magnitude of unevenness of the end surface of the coil based on the median value of the measurement values.

[0064] In the deriving step, the magnitude of the unevenness of the coil end surface does not have to be calculated using a two-dimensional coordinate system defined by the direction in which the unevenness of the coil end surface protrudes and the direction of scanning by the displacement meter. For example, in the deriving step, the measurement result by the displacement meter may be directly derived as the magnitude of the unevenness of the coil end surface. EXAMPLES

[0065] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0066] [No.1] A hot-rolled steel sheet was manufactured using the manufacturing equipment 1 shown in FIG. 2. First, the surface temperature of the strip steel X after hot rolling and before being wound by the winding machine 2c was measured over the entire area (total length and width) of the surface of the strip steel X using a non-contact temperature sensor 3a (thermography "CPA-SC7100" manufactured by FLIR) (measurement step). Next, the temperature history of the coil (virtual coil) in the natural cooling state, assuming that the strip steel X was wound into a coil shape without unevenness on the end surface, was calculated using the above formulas (2) to (5) (first calculation step). In this first calculation step, 10 calculation points were provided in the central axis direction of the imaginary coil and 50 points in the radial direction (total: 10 x 50 points), and the temperature history in the natural cooling state was calculated for each calculation point. FIG. 7 shows the temperature history in the natural cooling state based on the point immediately after winding of the upper end surface 410 mm away from the central axis of the imaginary coil in the radial direction.

[0067] Next, the strip steel X was actually wound by the winding machine 2c (winding process). Next, the end face E of the wound coil X1 was scanned over the diameter with a displacement meter 5b (a laser displacement meter "IL-2000" manufactured by KEYENCE Corporation), and the shape of the unevenness of the end face E of the coil X1 was measured. Furthermore, a reference plane of the end face E was set based on the median value of the measured values ​​by the displacement meter 5b, and the size of the unevenness of the end face E was derived by the derivation unit 5c using a two-dimensional coordinate system defined by the protruding direction of the unevenness and the scanning direction by the displacement meter 5b (deriving process). Note that the unevenness of the end face E of the coil X1 was positive when it protruded toward the displacement meter 5b, and negative when it was recessed toward the conveyor 5a. In this derivation process, the coil X1 was divided into 13 regions in the radial direction, the size of the unevenness was averaged for each region, and this average value was converted into a two-dimensional coordinate system to derive the size of the unevenness of this region. In this derivation process, the length of a pair of regions located at both ends in the radial direction was set to be smaller than the length of the other regions so that the unevenness caused by the telescope could be easily reflected. Specifically, the length of the regions located at both ends in the radial direction was set to 1 / 2 the length of the other regions. In addition, the unevenness threshold was set to 10 mm, and values ​​less than 10 mm were discarded for the average unevenness of each region. The measurement results of the shape of the unevenness of the end face E of the coil X1 by the displacement meter 5b in this derivation process and the derivation results of the magnitude of the unevenness of the end face E of the coil X1 by the derivation unit 5c are shown in FIG. 8.

[0068] Next, for the uneven portion of the end face E of the coil X1 derived in the derivation process, the temperature history in a cooling state based on the time immediately after winding was predicted using the calculation result in the first calculation process and the above formulas (2) to (5) (first prediction process). The prediction result in the first prediction process for the end face E of the coil X1 at a position 410 mm away from the central axis in the radial direction is shown in Fig. 9. Fig. 9 also shows the actual measurement value of the temperature 23 minutes after immediately after winding of the end face E of the coil X1 corresponding to the position predicted in the first prediction process.

[0069] [No.2] Using the same manufacturing equipment 1 as in No. 1, the measurement step, the first calculation step, the winding step, the derivation step, and the first prediction step were performed in the same manner as in No. 1. FIG. 10 shows the temperature history in a cooling state based on the point immediately after winding of the upper end face of the imaginary coil, which is 410 mm away from the central axis in the radial direction. FIG. 11 shows the measurement results of the shape of the unevenness of the end face E of the coil X1 by the displacement meter 5b in the derivation step, and the derivation results of the magnitude of the unevenness of the end face E of the coil X1 by the derivation unit 5c. FIG. 12 shows the prediction result by the first prediction step of the end face E of the coil X1 at a position 410 mm away from the central axis in the radial direction, and the actual temperature value 24 minutes after immediately after winding of the end face E of the coil X1 corresponding to the position predicted in the first prediction step.

[0070] 7 to 12, for both No. 1, which was determined to have unevenness in the derivation process, and No. 2, which was determined to have no unevenness, the prediction results in the first prediction process and the actual measured values ​​are approximately the same. This shows that the temperature history of the unevenness of the end face E of the coil X1 can be predicted sufficiently accurately for both No. 1 and No. 2.

[0071] [No.3] Using the same manufacturing apparatus 1 as in No.1, the measurement process, the first calculation process, the winding process, the drawing out process, and the first prediction process were performed. In addition, in No.3, the phase transformation rate of the end face of the coil was calculated using the above-mentioned formula (8) and formula (9), and the transformation heat value was calculated using the above-mentioned formula (10) (second calculation process). In No.3, the temperature history was predicted using the above-mentioned formula (6) and formula (7) in the first calculation process and the first prediction process. Furthermore, in No.3, the Vickers hardness [Hv] was measured at the position (calculation point) where the phase transformation rate was calculated in the second calculation process. The phase transformation rate calculated in No.3 and the Vickers hardness measured in No.3 are shown in Table 1.

[0072] [Table 1]

[0073] As shown in Table 1, the calculation point A with a small phase transformation rate has a larger Vickers hardness than the calculation points B and C with a large phase transformation rate. This shows that the phase transformation rate is correlated with the hardness of the coil. Therefore, by calculating the phase transformation rate in the second calculation step, the hardened part of the coil can be predicted. In addition, by setting a threshold value of the hardness or phase transformation rate at which the steel material may break in a subsequent process such as a cold rolling process, and comparing the calculated phase transformation rate with this threshold value, it is possible to predict whether or not the steel material will break in the subsequent process. [Industrial Applicability]

[0074] As described above, the method for producing a hot-rolled steel sheet according to one aspect of the present invention is suitable for detecting in advance the possibility of fracture of a steel material during the production of a cold-rolled sheet, etc. [Explanation of symbols]

[0075] 1. Hot-rolled steel sheet manufacturing equipment 2. Hot rolling equipment 2a Rolling mill 2b Conveyor section 2c winder 3. Measuring Equipment 3a Non-contact temperature sensor 4. Calculation device 5 Derivation device 5a Conveyor 5b Displacement gauge 5c Derivation part 6 Prediction Device 7 Cooling device X Steel strip X1 Coil X2 Virtual Coil E End face O Origin R Coil end reference surface Z Coil central axis

Claims

1. A measuring step of measuring a surface temperature of the hot-rolled steel strip; A first calculation step of calculating a temperature history in a cooling state after winding, assuming that the strip steel material is wound into a coil shape without unevenness on an end surface, based on the surface temperature measured in the measurement step; a winding process in which the strip steel material after the measuring process is actually wound into a coil; a deriving step of scanning an end surface of the coil wound in the winding step with a displacement meter and deriving the magnitude of unevenness of the end surface over a radius of the coil; a first prediction step of predicting a temperature history of the unevenness in a cooling state by using the temperature history calculated in the first calculation step and the magnitude of the unevenness derived in the derivation step; A method for manufacturing a hot-rolled steel sheet comprising the steps of:

2. a second calculation step of calculating a phase transformation rate using the temperature history predicted in the first prediction step; a second prediction step of predicting a hardened portion of the strip steel material using the phase transformation rate calculated in the second calculation step; The method for producing a hot-rolled steel sheet according to claim 1 , further comprising:

3. 3. The method for manufacturing a hot-rolled steel sheet according to claim 1 or 2, wherein in the deriving step, the magnitude of the unevenness is determined based on a median value of the measured values ​​by the displacement gauge.

4. 4. The method for manufacturing a hot-rolled steel sheet according to claim 1, 2 or 3, wherein the size of the irregularities is determined in the deriving step by using a two-dimensional coordinate system defined by a protruding direction of the irregularities and a scanning direction of the displacement gauge.

5. A measuring step of measuring a surface temperature of the hot-rolled steel strip; A first calculation step of calculating a temperature history in a cooling state after winding, assuming that the strip steel material is wound into a coil shape without unevenness on an end surface, based on the surface temperature measured in the measurement step; a winding process in which the strip steel material after the measuring process is actually wound into a coil; a deriving step of scanning an end surface of the coil wound in the winding step with a displacement meter and deriving the magnitude of unevenness of the end surface over a radius of the coil; a first prediction step of predicting a temperature history of the unevenness in a cooling state by using the temperature history calculated in the first calculation step and the magnitude of the unevenness derived in the derivation step; A method for predicting the temperature history of a hot-rolled steel sheet comprising:

6. A measuring step of measuring a surface temperature of the hot-rolled steel strip; A first calculation step of calculating a temperature history in a cooling state after winding, assuming that the strip steel material is wound into a coil shape without unevenness on an end surface, based on the surface temperature measured in the measurement step; a winding process in which the strip steel material after the measuring process is actually wound into a coil; a deriving step of scanning an end surface of the coil wound in the winding step with a displacement meter and deriving the magnitude of unevenness of the end surface over a radius of the coil; a first prediction step of predicting a temperature history of the unevenness in a cooling state by using the temperature history calculated in the first calculation step and the magnitude of the unevenness derived in the derivation step; a second calculation step of calculating a phase transformation rate using the temperature history predicted in the first prediction step; a second prediction step of predicting a hardened portion of the strip steel material using the phase transformation rate calculated in the second calculation step; A method for predicting hardened parts of a hot-rolled steel sheet comprising:

Citation Information

Patent Citations

  • Edge breakdown preventing method of hot rolled coil

    JP1999244939A

  • Method for cooling coil

    JP2005281809A

  • Telescoping amount calculation method of coil

    JP2010112958A

  • Temperature unevenness prediction method of hot rolled steel sheet, flatness control method, temperature unevenness control method and manufacturing method

    JP2014000593A

  • Apparatus and method of automatically callibrating telescope

    KR1020140084609A