Quartz glass body
The method of producing quartz glass bodies using silicon dioxide powder and multi-stage filtration in a controlled environment addresses impurity and cost issues, resulting in high-purity, high-temperature-resistant glass suitable for semiconductor applications.
Patent Information
- Application Number
- JP2023541696
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-01-21
- Filing Date
- 2022-01-17
- Publication Date
- 2024-11-28
- Estimated Expiration
- 2042-01-17
AI Technical Summary
Existing methods for producing quartz glass bodies suffer from impurities that lead to reduced efficiency, contamination, and high costs, particularly in applications like semiconductor manufacturing, where high purity and low OH content are required.
A method involving the use of silicon dioxide powder, sonicating a slurry to form a precursor suspension, passing it through multi-stage filters, and forming silicon dioxide granules before melting in a furnace with controlled gas dew points to produce high-purity quartz glass bodies.
The method results in quartz glass bodies with low impurities, high viscosity, and low OH content, suitable for high-temperature applications and semiconductor processing, while reducing production costs.
Smart Images

Figure 0007591661000017 
Figure 0007591661000018 
Figure 0007591661000019
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a quartz glass body, comprising the process steps of: i.) preparing a silicon dioxide powder and a liquid; ii.) mixing the liquid with silicon dioxide particles to obtain a slurry; iii.) treating the slurry with ultrasound to obtain a precursor suspension; iv.) passing the precursor suspension through a first multi-stage filter device to obtain a silicon dioxide suspension; v.) producing silicon dioxide granules from the silicon dioxide suspension; vi.) producing a glass melt from the silicon dioxide granules in a furnace; and vii.) producing a quartz glass body from at least a portion of the glass melt, wherein the treatment of the slurry in step iii.) comprises deagglomerating at least a portion of the silicon dioxide particles; and v.) producing a quartz glass body from at least a portion of the glass melt. the silicon dioxide granules have a particle size larger than the silicon dioxide particles contained in the silicon dioxide suspension, the furnace has a crucible and a gas vent for removing gas from the furnace, the dew point of the gas leaving the furnace through the gas vent is less than 0 ° C, the first multi-stage filter device has at least a first, a second and a third filter stage, the second filter stage is arranged downstream of the first filter stage, the third filter stage is arranged downstream of the second filter stage, each filter stage comprises at least one filter, the first filter stage has a filter fineness of 5 μm or more, the second filter stage has a filter fineness in the range of 0.5 to 5 μm, and the third filter stage has a filter fineness of 1 μm or less, the filter fineness indicating the minimum particle size retained by the filter, in each case according to ISO The separation rate for the first filter stage is 50% or more, the separation rate for the second filter stage is 95% or more, and the separation rate for the third filter stage is 99.5% or more as specified in 16889. The present invention also relates to a quartz glass body obtainable from this method, as well as a light guide, a light emitter, an apparatus and a molding.
[0002] Quartz glass, quartz glass products and products containing quartz glass are known.Various methods for producing quartz glass and quartz glass bodies are already known.Nevertheless, there are still great efforts being made to identify preparation processes that can prepare quartz glass with higher purity, i.e., without impurities.
[0003] In many fields of application of quartz glass and its processed products, high requirements are made, for example, with respect to homogeneity and purity. This applies in particular to quartz glass that is processed into light guides or illuminators. In this case, impurities can cause absorption, which is disadvantageous because it attenuates the emitted light.
[0004] UV lights and their jacket tubes are used, for example, for water disinfection or air and surface disinfection. The purpose is to emit UV radiation in a given wavelength range where impurities reduce the efficiency of irradiation. For this reason, products with and / or of synthetic quartz glass are particularly preferred. However, to be competitive in this market, quartz glass products must be inexpensive. Therefore, existing methods for making synthetic quartz glass products are not marketable.
[0005] A further example of the use of high purity quartz glass is the manufacturing step in semiconductor manufacturing. Here, any impurities in the glass body can potentially lead to defects in the semiconductor, which is therefore rejected during manufacturing. As in semiconductor manufacturing, developments have led to narrower and narrower structure widths, higher packaging densities, stacking, with an increased number of process steps on the wafer and the use of larger wafers as substrates, and the concern regarding impurities has obviously increased. At the same time, reject costs have risen disproportionately. For these reasons, there is a need for reactors and manufacturing devices that can minimize the transfer of contamination to the wafer as much as possible.
[0006] For these reasons, industry is showing great interest in synthetic quartz glass reactors and devices, where previously quartz glass from natural sources was used. The high purity quartz glass types used in these processes, especially the high purity synthetic quartz glass types, are very expensive to make. They are expensive. Nevertheless, the demand here is considerable. Summary of the Invention [Problem to be solved by the invention]
[0007] However, in some applications, synthetic quartz glass has drawbacks, especially for reactors and devices in semiconductor manufacturing. For example, the absence of certain metal ions, especially aluminum, makes synthetic quartz glass less viscous than natural quartz glass. On the other hand, it has relatively more OH groups, which result from the production of silicon dioxide, especially by flame hydrolysis. This results in a lower viscosity and therefore reduces the maximum temperature at which they can be used compared to natural quartz glass.
[0008] On the other hand, synthetic quartz glass with fewer OH groups can be produced by treating the precursor stage (for example, the porous body or the granulation from nanoparticles) with chlorine, hydrochloric acid, etc., before the melting step. This removes the OH groups. However, the quartz glass thus obtained is then contaminated with chlorine and has a low viscosity, which precludes certain applications. The semiconductor industry is also concerned that chlorinated quartz glass reactors release chlorine, which can react with other metals and contaminate the wafer or corrode structures established on the wafer. It is therefore desirable that synthetic quartz glass, like natural quartz glass, not only has fewer OH groups, but also does not contain chlorine and can have a high viscosity.
[0009] Since the market desires high purity quartz glass, and in particular high purity synthetic quartz glass and products already mentioned above, it would be highly attractive to be able to produce synthetic quartz glass of good quality comparable to said high purity quartz glass, while at the same time offering them at a lower price than the quartz glass grades currently known on the market. With this in mind, there is a demand for both cheaper manufacturing processes and cheaper sources of raw materials.
[0010] Known processes for making quartz glass bodies include melting silicon dioxide and forming a quartz glass body from the melt. Irregularities in the glass body, for example due to trapped gas in the form of bubbles, can cause the glass body to break under stress, especially at high temperatures, or prevent it from being used for a particular purpose. For example, if the raw materials used in making quartz glass are contaminated, this can result in cracks, bubbles, strips and discoloration forming in the quartz glass.
[0011] When used in processes for making and processing semiconductor components, contaminants in the glass body can leach out and migrate to the processed semiconductor components. This is the case, for example, in etching processes, leading to breakage of the semiconductor blank. If gas inclusions are present, they will leach out and form particles in the etching processes used in semiconductor manufacturing. This is also considered dangerous. Thus, a problem that often occurs in known manufacturing processes is that the quality of the quartz glass body used is insufficient.
[0012] Another aspect is raw material efficiency. It seems advantageous to use quartz glass and raw materials that occur as by-products elsewhere that are industrially processed to make quartz glass products, instead of simply using these by-products as fillers, for example in construction, or disposing of them as waste at high cost. These by-products are often trapped in filters as fine dust. This fine dust creates additional problems, especially in terms of health, safety at work and handling.
[0013] assignment One object of the present invention is to overcome, in particular in part, one or more disadvantages arising from the prior art.
[0014] It is a further object of the present invention to provide light guides, illuminators, moldings and coatings that have a long life.
[0015] It is a further object of the present invention to provide light guides, shaped illuminators, objects and coatings made from glasses that are bubble-free or have a low bubble content.
[0016] It is a further object of the present invention to provide light guides, illuminators, moldings and coatings made from glass having a high degree of transparency.
[0017] It is a further object of the present invention to provide light guides, illuminators, moldings and coatings that have low opacity.
[0018] It is a further object of the present invention to provide a light guide with low attenuation.
[0019] It is a further object of the present invention to provide light guides, light emitters, moldings and coatings with high contour accuracy. In particular, it is an object of the present invention to provide light guides, light emitters, moldings and coatings that do not deform at high temperatures. In particular, it is an object of the present invention to provide light guides, light emitters, moldings and coatings that are shape-stable even when formed in large sizes.
[0020] It is a further object of the present invention to provide light guides, illuminators, moldings and coatings that are tear and puncture resistant.
[0021] It is a further object of the present invention to provide light guides, illuminators, moldings and coatings that are efficient to prepare.
[0022] It is a further object of the present invention to provide light guides, illuminators, moldings and coatings that are cost-effective to prepare.
[0023] It is a further object of the present invention to provide light guides, luminophores, moldings and coatings, the preparation of which does not require lengthy further processing steps, such as tempering.
[0024] It is a further object of the present invention to provide light guides, illuminators, moldings and coatings that have high thermal shock resistance, in particular light guides, illuminators, moldings and coatings that exhibit only low thermal expansion with large thermal fluctuations.
[0025] It is a further object of the present invention to provide light guides, illuminators, moldings and coatings which have a high hardness.
[0026] It is a further object of the present invention to provide light guides, illuminators, moldings and coatings which are highly pure and substantially free of foreign atom contamination, "foreign atom" being understood to mean components which are not intentionally introduced.
[0027] It is a further object of the present invention to provide light guides, phosphors, moldings and coatings which contain a low content of dopant material.
[0028] It is a further object of the present invention to provide light guides, illuminators, moldings and coatings having a high degree of homogeneity. The homogeneity of a property or material is a measure of the uniformity of the distribution of this property or material in a sample.
[0029] In particular, it is an object of the present invention to provide light guides, light emitters, moldings and coatings with high material homogeneity, which is a measure of the uniformity of the distribution of elements and compounds, in particular OH, chlorine, metals, in particular aluminum, alkaline earth metals, refractory metals and dopant materials, contained in the light guide, light emitter or semiconductor device.
[0030] It is a further object of the present invention to provide light guides, illuminators, moldings and coatings made from glasses whose glass bodies do not attenuate light intensity in the visible range.
[0031] A further object of the invention is to provide light guides, luminaries, mouldings and coatings made from glasses whose glass bodies attenuate radiation in the IR range as little as possible.
[0032] It is a further object of the present invention to provide light guides, illuminators, moldings and coatings made from glass, the glass body of which is translucent to light in the IR range.
[0033] It is a further object of the present invention to provide light guides, luminaries, moldings and coatings made from glasses whose glass bodies do not absorb light.
[0034] It is a further object of the present invention to provide coatings made from non-fluorescent light guides, illuminators, moldings and glasses.
[0035] In particular, it is an object of the present invention to provide light guides, luminescent bodies, mouldings and coatings made from glasses which do not fluoresce when excited with radiation in the UV range, in particular with wavelengths of 254 nm or 365 nm or both.
[0036] It is a further object of the present invention to provide light guides, luminescent bodies, moldings and coatings made from glasses with a defined OH content, which can contribute to equalizing structural changes in quartz glass induced by radiation such as UV, i.e. to compensating for so-called radiation damage.
[0037] It is a further object of the present invention to provide light guides, luminescent bodies, moldings and coatings made from glasses having a defined OH content in the range of 100-200 ppm.
[0038] It is a further object of the present invention to provide reactors, guides, bodies and coatings that are particularly suited for certain process steps in semiconductor manufacturing, especially wafer fabrication. Examples of such process steps are plasma etching, chemical etching and plasma.
[0039] It is a further object of the present invention to provide reactors, guides, compacts and coatings which, when used in semiconductor manufacturing, particularly wafer fabrication, help minimize rejects during semiconductor fabrication.
[0040] It is a further object of the present invention to provide light guides, luminophores, moldings and coatings which contain little or no metal ions.
[0041] It is an object of the present invention to provide light guides, luminescent bodies, moldings and coatings which contain as few atoms other than Si, O and possibly H as possible.
[0042] It is a further object of the present invention to provide light guides, illuminators, moldings and coatings which can be used at high operating temperatures.
[0043] It is a further object of the present invention to provide light guides, illuminators, moldings and coatings which are stable even when used at high temperatures, in particular light guides, illuminators and components which do not emit particles during operation.
[0044] A further object of the present invention is to provide a quartz glass body which is suitable for use in light guides, luminescent bodies, moldings and coatings on quartz glass and which at least partially solves at least one, preferably more, of the problems already described.
[0045] A further object of the present invention is to provide a quartz glass body having a linear design. In particular, it is an object of the present invention to provide a quartz glass body having a high bending radius. In particular, it is an object of the present invention to provide a quartz glass body having a high curl parameter.
[0046] A further object is to provide a quartz glass body in which cation migration is as low as possible.
[0047] A further object is to provide a quartz glass body which is as homogeneous as possible over its entire length.
[0048] In particular, an object of the present invention is to provide a quartz glass body having a high refractive index over its entire length.
[0049] In particular, it is an object of the present invention to provide a quartz glass body which is very homogeneously viscous over its entire length.
[0050] In particular, it is an object of the present invention to provide a quartz glass body having high material homogeneity over its entire length.
[0051] In particular, it is an object of the present invention to provide a quartz glass body that is highly optically homogeneous over its entire length.
[0052] A further object of the present invention is to provide a quartz glass body having a defined OH content.
[0053] A further object of the present invention is to provide a quartz glass body having a low OH content.
[0054] A further object of the present invention is to provide a quartz glass body having a high viscosity.
[0055] A further object of the present invention is to provide a quartz glass body which can be used at as high temperatures as possible.
[0056] A further object of the present invention is to provide a quartz glass body having a low OH content.
[0057] A further object of the present invention is to provide a quartz glass body that contains little or no chlorine. A further object of the present invention is to provide a quartz glass body that is less contaminated by the crucible material.
[0058] In particular, it is an object of the present invention to provide a quartz glass body having a low content of metal contaminants.
[0059] In particular, it is an object of the present invention to provide a quartz glass body having a low tungsten content.
[0060] In particular, a further object of the present invention is to provide a quartz glass body having a low molybdenum content.
[0061] A further object of the present invention is to produce a quartz glass body that has little or no contamination from the inner crucible material, in particular tungsten and molybdenum.
[0062] A further object of the present invention is to provide a quartz glass body that has low OH, low chlorine, low metal contaminants, and at the same time has high viscosity, high temperature stability, and can be used at high temperatures.
[0063] A further object of the present invention is to provide a quartz glass body that has low OH, low chlorine, and as low as possible metal contaminants, and at the same time has high viscosity, high temperature stability, can be used at high temperatures, and can be produced more cheaply than other synthetic quartz glasses.
[0064] A further object of the present invention is to provide a quartz glass body that has almost no OH groups, as little or no chlorine as possible, and as little or as little metal components as possible. At the same time, the quartz glass body should have a high viscosity, high temperature stability, be usable at high temperatures, and can be produced at the same cost, more cheaply, or if possible, less expensively than natural quartz glass.
[0065] A further object of the present invention is to provide a quartz glass body and subsequent products therefrom, such as light guides, luminous bodies, moldings, coatings, reactors, guides, etc., which, in some cases, do not fluoresce when irradiated with light in the UV range, in particular with wavelengths of 254 nm or 365 nm, and which also have few OH groups and, if possible, contain little or no chlorine. In addition, such quartz glass bodies and subsequent products should be able to be used at high temperatures and have high viscosity. It is also an object of the present invention to provide a quartz glass body having a combination of two or more of the above-mentioned properties.
[0066] A further object of the present invention is to make it possible to produce a quartz glass body which at least partially solves at least some of the problems already mentioned above.
[0067] A further object of the present invention is to provide a process by which the quartz glass body can be prepared more simply.
[0068] A further object of the present invention is to provide a process by which a quartz glass body can be continuously prepared.
[0069] A further object of the present invention is to provide a process by which a quartz glass body can be prepared by a continuous melting and forming process.
[0070] A further object of the present invention is to provide a process capable of forming a quartz glass body at high speed.
[0071] A further object of the present invention is to provide a process capable of preparing a quartz glass body with a low rejection rate.
[0072] A further object of the present invention is to provide a process by which a tunable quartz glass body can be prepared.
[0073] A further object of the present invention is to provide an automated process capable of preparing a quartz glass body.
[0074] A further object of the present invention is to provide a process for the preparation of a quartz glass body in which the silicon dioxide granules can be processed in a melting furnace without the need to previously subject them to an intentional compression step, for example by temperature treatment above 1000 ° C.
[0075] In particular, the subject of the present invention is 2 The object of the present invention is to provide a process for preparing a quartz glass body, which can be obtained by introducing silicon dioxide granules having a BET of 1.0 to 1.0 g / g or more into a melting furnace, melting and processing the same to obtain a quartz glass body.
[0076] A further object of the present invention is to provide a process for the preparation of a quartz glass body, the components of which have as long a service life as possible under the process conditions.
[0077] In particular, it is an object of the present invention to provide a process for the preparation of quartz glass bodies in which furnace corrosion is avoided.
[0078] A further object of the present invention is to provide a process for the preparation of a quartz glass body, which can use silicon dioxide raw material having a high residual moisture. "Silicon dioxide raw material" means, for example, silicon dioxide granules.
[0079] In particular, the object of the present invention is to provide a process for the preparation of a quartz glass body, in which a silicon dioxide input material having a high residual moisture can be used without a pretreatment step.
[0080] In particular, a further object of the present invention is to provide a process for the preparation of a quartz glass body in which a silicon dioxide input material having a high residual moisture can be used in a system having a melting crucible of refractory metal.
[0081] A further object of the present invention is to provide a process for the preparation of glass bodies, the components of which have as long as possible a service life under the process conditions.
[0082] A further object of the present invention is to provide a process for the preparation of a glass body having a defined OH content.
[0083] A further object of the present invention is to provide a process for the preparation of a quartz glass body having a low OH content.
[0084] A further object of the present invention is to provide a process for the preparation of a quartz glass body having a defined content of ODC (oxygen deficient centers).
[0085] A further object of the present invention is to provide a process for the preparation of a quartz glass body having a high content of ODC (oxygen deficient centers).
[0086] A further object of the present invention is to provide a process for the preparation of a quartz glass body having a low input of impurities from the furnace.
[0087] A further object of the present invention is to provide a process for the preparation of a quartz glass body, which can process hygroscopic silicon dioxide granules without reducing the service life of the crucible, especially if the crucible is hardly corroded.
[0088] A further object of the present invention is to provide a process for the preparation of a quartz glass body with low gas consumption. In particular, it is an object of the present invention to provide a process for producing a quartz glass body with low helium consumption. In particular, it is an object of the present invention to provide a process for the preparation of a quartz glass body with low hydrogen consumption.
[0089] A further object of the present invention is to provide a process for the preparation of a quartz glass body, in which the quartz glass body and any subsequent products made therefrom do not emit fluorescence when irradiated with UV light, in particular at wavelengths of 254 nm or 365 nm, have few OH groups, and contain as little or no chlorine as possible. Furthermore, such quartz glass bodies and subsequent products should be usable even at high temperatures and high viscosities.
[0090] A further object of the invention is to provide a process for the preparation of high-purity quartz glass.
[0091] A further object of the invention is to provide a process for the preparation of quartz glass containing as few bubbles as possible.
[0092] A further object of the present invention is to provide a process for the preparation of quartz glass which is free of particles of metal contaminants.
[0093] A further challenge is to continue to improve the processability of quartz glass bodies.
[0094] A further challenge is to continue to improve the adjustability of the quartz glass body.
[0095] The present invention is based on the realization that it is possible to produce quartz glass with certain characteristics and with significantly improved quality by using only a combination of several measures.In this process, silicon dioxide powder and even soot powder, i.e. by-products or waste products obtained from other glass synthesis, can be used to prepare high-quality quartz glass that is comparable to other high-quality synthetic quartz glass products.It is particularly free of gas inclusions or contamination by foreign atoms, i.e. atoms other than silicon and oxygen.The combination of measures includes adding silicon components other than silicon dioxide, such as silicon, filtering the formed silicon dioxide suspension as an intermediate step, and monitoring the dew point of the gas flow leaving the crucible.
[0096] By varying a single parameter, the main properties of the quartz glass body that can be prepared using the amount of silicon components other than silicon dioxide can be controlled, including its viscosity, the appearance and extent of absorption of electromagnetic radiation in the UV range, the appearance and extent of absorption of electromagnetic radiation in the IR range, or some combination of such properties.
[0097] As far as the process step of melting the granulation to obtain a glass melt is concerned, the addition of silicon can also be used to control the amount of OH groups and / or hydrogen molecules in the crucible, so as to avoid corrosion of the crucible and thus possible contamination of the glass melt. The situation in the crucible can be effectively controlled by determining the dew point of the gas emanating from the crucible. Here again, no foreign atoms, i.e. atoms other than silicon and oxygen, are introduced into the resulting quartz glass.
[0098] The above silicon dioxide powder can be used to produce high quality quartz glass, and its quality can be compared with other synthetic quartz glass products of similar quality when the soot powder is first processed through a slurry to produce granulation, and the slurry is passed through a filtration system before granulation. This process contributes greatly to avoid gas bubbles that form due to contaminants that can be oxidized into gas and gas contents.
[0099] EMBODIMENTS OF THE PRESENT DISCLOSURE A contribution to achieving at least one of the above mentioned objectives is made by the subject matter of the independent claims. The dependent claims are preferred embodiments which contribute to at least partially fulfilling at least one of the objectives.
[0100] |1| A method for producing a quartz glass body, i.) providing a powder of silicon dioxide particles and providing a liquid; ii.) mixing the powder with a liquid to obtain a slurry containing the liquid and silicon dioxide particles; iii.) treating the slurry with ultrasound to obtain a precursor suspension; iv.) passing at least a portion, and preferably all, of the total precursor suspension through at least a first multi-stage filter device to obtain a silicon dioxide suspension; v.) forming silicon dioxide granules from the silicon dioxide suspension, preferably by spray drying; vi.) forming a glass melt from the silicon dioxide granules in a furnace; vii.) forming a quartz glass body from at least a portion of the glass melt; The process steps include Treating the slurry in step iii.) includes deagglomerating at least a portion of the silicon dioxide particles; Step v.) comprises granulation, The silicon dioxide granules have a particle size larger than the silicon dioxide particles contained in the silicon dioxide suspension, The furnace has a crucible and a gas outlet; Gas is removed from the furnace via a gas outlet, The dew point of the gas leaving the furnace through the gas outlet is below 0°C; the first multi-stage filter device has at least first, second and third filter stages; a second filter stage disposed downstream of the first filter stage, and a third filter stage disposed downstream of the second filter stage; Each filter stage includes at least one filter; the first filter stage has a filter fineness of 5 μm or more, the second filter stage has a filter fineness in the range of 0.5 to 5 μm, and the third filter stage has a filter fineness of 1 μm or less; Filter fineness indicates the smallest particle size that the filter will retain; The separation rate for the first filter stage as specified by ISO 16889 in each case is 50% or more, for the second filter stage 95% or more and for the third filter stage 99.5% or more.
[0101] |2| The method according to embodiment 1, wherein the granulation is selected from the group consisting of rotary granulation, spray granulation, centrifugal atomization, freeze granulation and fluidized bed granulation.
[0102] |3| The method according to one of the above embodiments, wherein a silicon component other than silicon dioxide is added in at least one of the process steps.
[0103] |4| The method according to one of the above embodiments, wherein the silicon component other than silicon dioxide is silicon, a silicon-hydrogen compound, a silicon-oxygen compound or a silicon-hydrogen-oxygen compound, particularly preferably silicon.
[0104] |5| The method according to one of the above embodiments, wherein the silicon component is added as a powder.
[0105] |6| The method according to one of the above embodiments, wherein the silicon component is added as a liquid or a gas.
[0106] |7| The method according to one of the above embodiments, wherein a silicon component other than silicon dioxide is added in one of steps i.), ii.) or v.), or between two or more of said steps, particularly preferably during step v.).
[0107] |8| The method according to any one of embodiments |3| to |7|, wherein the one or more silicon components other than silicon dioxide are added in a total amount of 10 to 100,000 ppm, in ppm based on the total weight of silicon dioxide.
[0108] |9| The method according to one of the above embodiments, wherein forming the granulation in step v.) comprises spray-drying the silicon dioxide suspension formed in step iv.), the spray-drying being carried out by spraying the silicon dioxide suspension through a nozzle in a spray tower, the spray-drying being characterized by at least one of the following characteristics: a] Spray granulation in a spray tower; b] the silicon dioxide suspension in the nozzle is pressurized to less than 40 bar, for example in the range from 1.3 to 20 bar or from 1.5 to 18 bar, or from 2 to 15 bar or from 4 to 13 bar, or particularly preferably in the range from 5 to 12 bar, the stated pressures being absolute pressures (based on p=0 hPa); c] when the droplets enter the spray tower, their temperature is in the range of 10-50 ° C, preferably in the range of 15-30 ° C, particularly preferably in the range of 18-25 ° C; d] the temperature on the side of the nozzle facing the spray tower is in the range from 100 to 450 ° C, for example in the range from 250 to 440 ° C, particularly preferably from 350 to 430 ° C; e] The throughput of the silicon dioxide suspension passing through the nozzle is 0.05 to 1 m 3 / h range, e.g. 0.1~0.7m 3 / h or 0.2~0.5m 3 / h, and particularly preferably 0.25 to 0.4 m 3 / h range; f] the silicon dioxide suspension has a solids content of at least 40% by weight, for example in the range from 50 to 80% by weight or in the range from 55 to 75% by weight, particularly preferably in the range from 60 to 70% by weight, in each case based on the total weight of the silicon dioxide suspension a; g] gas flows into the spray tower in the range of 10-100 kg / min, for example in the range of 20-80 kg / min or 30-70 kg / min, particularly preferably in the range of 40-60 kg / min; h] the gas enters the spray tower at a temperature in the range of 100-450 ° C, for example in the range of 250-440 ° C, particularly preferably 350-430 ° C; i] The gas leaves the spray tower at a temperature below 170°C; j] the gas is selected from the group consisting of air, nitrogen and helium or a combination of two or more thereof, preferably air; k] the granules removed from the spray tower have a residual moisture of less than 5%, for example less than 3% by weight or less than 1% by weight or in the range from 0.01 to 0.5% by weight, particularly preferably in the range from 0.1 to 0.3% by weight, in each case based on the total weight of the silicon dioxide granules obtained by spray drying; l] at least 50 wt.-% of the spray granules, based on the total weight of the silicon dioxide granules obtained by spray drying, completes a flight time in the range of 1 to 100 seconds, for example over a period of 10 to 80 seconds, particularly preferably over a period of 25 to 70 seconds; m] At least 50 wt.-% of the spray granules, based on the total weight of the silicon dioxide granules obtained by spray drying, fly within more than 20 m, for example more than 30 m or more than 50 m or more than 70 m or more than 100 m or more than 150 m or more than 200 m or in the range from 20 to 200 m or from 10 to 150 or from 20 to 100 m, particularly preferably in the range from 30 to 80 m; n] the spray tower has a cylindrical shape; o] the spray tower has a height of more than 10 m, for example more than 15 m or more than 20 m or more than 25 m or more than 30 m, or in the range from 10 to 25 m, particularly preferably in the range from 15 to 20 m; p] Screening particles less than 90 μm in size before removing the granulation from the spray tower; q] After removing the granulation from the spray tower, particles with a size of more than 500 μm are filtered off, preferably on a vibrating table; r] The silicon dioxide suspension droplets emerge from the nozzle at an angle of 30 to 60° to the vertical, particularly preferably at an angle of 45° to the vertical.
[0109] |10| The method according to one of the above embodiments, wherein the melt energy impinges on a fixed surface of the silicon dioxide granules.
[0110] |11|A method according to one of the above embodiments, wherein the dew point of the gas before entering the furnace is at least 30° C. lower than the dew point when it leaves the furnace through the gas outlet.
[0111] |12|The method according to one of the above embodiments, wherein the melting furnace is at least partially made of a material containing one or more metals selected from molybdenum, tungsten, rhenium, iridium and osmium.
[0112] |13| The method according to one of the above embodiments, wherein the quartz glass body contains less than 1000 ppb in total of one or more metals selected from molybdenum, tungsten, rhenium, iridium and osmium, the total amount being based on the total weight of the quartz glass body.
[0113] |14| The method according to one of the above embodiments, wherein the dew point is determined in a test cell, the test cell being separated by a membrane from the gas flow exiting the gas outlet.
[0114] |15|The method according to one of the above embodiments, wherein a dew point level hygrometer is used to determine the humidity level.
[0115] |16|The method according to any one of the preceding embodiments, wherein the furnace gas space contains hydrogen, helium, nitrogen, or a combination of two or more thereof.
[0116] |17| The method according to one of the above embodiments, wherein the silicon dioxide powder can be made from a compound selected from the group consisting of siloxanes, silicon alkoxides and silicon halides.
[0117] |18|The method according to one of the above embodiments, wherein the first filter device is characterized by at least one of the following characteristics: (a) the first filter stage has a filter fineness of 5 μm or more, for example, 5 μm to 15 μm; (b) the first filter stage has a separation efficiency of 90% or less, e.g., in the range of 50-90%; (c) the second filter stage has a filter fineness of 0.5 μm or more, for example in the range of 0.5 to 10 μm; (d) the second filter stage has a separation efficiency of 80% or greater, such as 99.5% or greater. (e) the third filter stage has a filter fineness of 0.5 μm or more, for example in the range of 0.5 μm to 10 μm or 0.1 μm to 1 μm; (f) the third filter stage has a separation ratio of 80% or more, e.g., 99.5% or more; Or a combination of at least two of characteristics (a) to (f).
[0118] |19|A method according to one of the above embodiments, wherein at least one filter in one of the filter stages of the first filter device selected from the first, second and third filter stages is designed as a depth filter.
[0119] |20| The method according to any of the above embodiments, wherein the slurry is treated with ultrasound for at least 10 seconds.
[0120] |21|A method according to one of the above embodiments, wherein the slurry is treated with ultrasound at a power density of up to 600 W / liter.
[0121] |22|The method according to one of the above embodiments, wherein the slurry has less than 5 wt. % based on the total weight of the slurry of additives to stabilize the slurry.
[0122] |23| The method according to one of the above embodiments, wherein the silicon dioxide powder has at least one of the following characteristics: a.Maximum 35m 2 / g, e.g. 25~35m 2 / g or 20~35m 2 / g or 25~30m 2 / g range of BET surface area; and b.0.01~0.3g / cm 3 Bulk density in the range of; c. Carbon content less than 100 ppm; d. Chlorine content less than 500 ppm; e. Aluminum content less than 200 ppb; f. Content of atoms other than Si, O, H, C, and Cl less than 5 ppm; g. at least 70% by weight of the powder particles have a primary particle size in the range of 10 to 100 nm; h.0.001~0.3g / cm 3 Tap density in the range of; i. less than 5% by weight residual moisture; j. Particle size distribution D in the range of 1 to 7 μm 10 ; k. Particle size distribution D in the range of 6 to 15 μm 50 ; l. Particle size distribution D in the range of 10 to 40 μm 90 ; or a combination of two or more of characteristics a.-l.; Here, the weight percentages are in each case based on the total amount of silicon dioxide powder.
[0123] Particle size distribution of silicon dioxide powder D 10 , D 50 and D. 90 is measured on a Mastersizer 2000 measured by laser refraction according to method x.
[0124] |24| The method according to one of the above embodiments, wherein the slurry has at least one of the following characteristics: A.) A solids content of at least 20% by weight based on the dry weight of the slurry; B.) As a 4 wt% slurry, the slurry has a pH value in the range of 3 to 8; C.) At least 90% by weight of the silicon dioxide particles have a particle size in the range of 1 nm to <100 μm; D.) The chlorine atom content is 500 ppm or less; E.) 5% content of atoms other than Si, O, H, C, and Cl; F.) The slurry is rheopectic; Wherein weight percent and ppm are always based on the total solids content of the slurry; G.) The slurry is conveyed in contact with a plastic surface; H.) The slurry is sheared; I.) The slurry has a temperature above 0°C, preferably in the range of 5 to 35°C; J.) the slurry has a viscosity according to DIN 53019-1 (5 rpm, 30% by weight) in the range from 500 to 2000 mPas, for example in the range from 600 to 1700 mPas, particularly preferably in the range from 650 to 1350 mPas; K.) In a 4 wt.% slurry, at least 5% of the silicon dioxide particles have a particle size according to DIN ISO 13320-1 in the range of >10 μm.
[0125] |25| The method according to one of the above embodiments, wherein the silicon dioxide suspension has at least one of the following characteristics: A. Rheopectic properties at temperatures below 45°C and solids concentrations in the range of 20-70 wt%, where wt% is based on the total solids in the suspension; B. at least 90 wt.-% of the silicon dioxide particles, based on the total weight of all silicon dioxide particles, have a particle size in the range of 1 nm to <10 μm, where the wt.-% is based on the solids content of the silicon dioxide suspension according to DIN ISO 13320-1; C. a pH value ranging from 3 to 8, where the pH value is based on a silicon dioxide suspension set at a solids content of 4% by weight; D. Chlorine content less than 500 ppm; E. Aluminum content less than 200 ppb; F. Content of atoms other than Si, O, H, C, Cl less than 5 ppm; G. Temperatures above 0°C, preferably in the range of 5-35°C; H. Viscosity according to DIN 53019-1 (5 rpm, 30% by weight) in the range from 500 to 2000 mPas, for example in the range from 600 to 1700 mPas, particularly preferably in the range from 650 to 1350 mPas; Here, ppm and ppb are in each case based on the total amount of silicon dioxide particles in the suspension.
[0126] |26|The method according to one of the above embodiments, wherein the service life of the first multi-stage filter is at least 250 liters, where liters is based on the filtered volume of the precursor suspension filter device.
[0127] |27|The method according to one of the above embodiments, wherein at least one further filter device is used downstream of the first multi-stage filter device.
[0128] |28| The method according to one of the above embodiments, wherein the silicon dioxide granules formed in step v.) have at least one of the following characteristics: [A] 20~50m 2 BET surface area in the range of / g; [B] average particle size in the range of 180-300 μm; [C] 0.5~1.2g / cm 3 Bulk density in the range of; [D] Carbon content less than 50 ppm; [E] Aluminum content less than 200 ppb; [F] 0.5~1.3g / cm 3 Tap density of; [G] Pore volume in the range of 0.1-1.5 ml / g; [H] Chlorine content less than 200 ppm; [I] Content of metals other than aluminum less than 1000 ppb; [J] Residual moisture less than 10% by weight; [K] Particle size distribution D in the range of 50-150 μm 10 ; [L] Particle size distribution D in the range of 150-300 μm 50 ; [M] Particle size distribution D in the range of 250-620 μm 90 ; [N] bulk angle in the range of 23-29°; Here, weight percent, ppm and ppb are in each case based on the total weight of the silicon dioxide granules.
[0129] |29| The method according to one of the above embodiments, wherein the silicon dioxide granules obtained in step v.) are subjected to a heat treatment before step vi.), and the resulting treated silicon dioxide granules have at least one of the following characteristics: (A) 10~35m 2 BET surface area in the range of / g; (B) average particle size in the range of 100–300 μm; (C) 0.7~1.2g / cm 3 Bulk density in the range of; (D) a carbon content of less than 5 ppm; (E) An aluminum content of less than 200 ppb; (F) 0.7~1.2g / cm 3 Tap density in the range of; (G) pore volume in the range of 0.1-2.5 ml / g; (H) Chlorine content less than 500 ppm; (I) A metal content of metals other than aluminum of less than 1,000 parts per billion; (J) less than 3% by weight residual moisture; (K) Particle size distribution D in the range of 50 to 150 μm 10 ; (L) Particle size distribution D in the range of 150 to 250 μm 50 ; (M) Particle size distribution D in the range of 250 to 450 μm 90 ; (N) bulk angle in the range of 23°-29°; Here, weight percent, ppm and ppb are in each case based on the total weight of the silicon dioxide granules.
[0130] |30| A quartz glass body having the following characteristics: A] Chlorine content less than 60 ppm; B] aluminum content less than 200 ppb; C] content of atoms other than Si, O, H, and C less than 5 ppm; D]log 10 (η(1250℃) / dPas)=11.4~log 10 (η(1250℃) / dPas)=12.9, or log 10(η(1300℃) / dPas)=11.1~log 10 (η(1300℃) / dPas)=12.2, or log 10 (η(1350℃) / dPas)=10.5~log 10 Viscosity in the range of (η(1350 °C) / dPas) = 11.5 (p = 1013 hPa); E]10 -4 Refractive index homogeneity of less than ; F] cylindrical; G] Tungsten content less than 100 ppb; H] molybdenum content less than 100 ppb; Here, ppb and ppm are in each case based on the total weight of the quartz glass body.
[0131] |31| A quartz glass body obtained by the method according to any one of the embodiments |1| to |29|.
[0132] |32|A quartz glass body according to embodiment |31|, characterized by at least one characteristic of embodiment |30|.
[0133] |33| A method for making a light guide, comprising the steps of: A / Providing a quartz glass body according to one of the embodiments |30| to |32| or using the method according to claim 1 to obtain a quartz glass body, the quartz glass body being first processed to obtain a hollow body having at least one opening; B / inserting one or more core rods into the hollow body from step A / through at least one opening to obtain a precursor; C / Thermally stretching the precursor to obtain a light guide having one or more cores and a jacket M1.
[0134] |34| A light guide obtainable by the method according to embodiment 33.
[0135] |35| A method for producing a luminous body, comprising the steps of: (i) providing a quartz glass body according to one of the embodiments |30| to |32| or carrying out the method according to claim 1 to obtain a quartz glass body, comprising first processing the quartz glass body into a hollow body having at least one opening; (ii) if necessary, attaching electrodes to the hollow body; (iii) filling the hollow body from step (i) with a gas;
[0136] |36| A phosphor obtainable by the method according to embodiment 35.
[0137] |37| A method for producing a molded body, comprising the steps of: (1) providing a quartz glass body according to any one of the embodiments |30| to |32| or carrying out the method according to claim 1 to obtain a quartz glass body; and (2) A step of forming the quartz glass body to obtain a formed body.
[0138] |38| A molded body obtainable by the method according to embodiment 37.
[0139] General Notes In this specification, ranges are inclusive of the values stated as limits. Thus, a description of the type "in the range from x to y" for a variable a means that a can take on values x, y, and values between x and y. A range limited on one side of the type "up to y" for a variable a means y and less than y.
[0140] Detailed Description of the Invention The independent claims contribute to at least partially satisfying at least one of the above stated objectives. The dependent claims present preferred embodiments which contribute to at least partially satisfying at least one of the objectives.
[0141] The first object of the present invention is to provide a method for producing a quartz glass body, i.) preparing a powder of silicon dioxide particles and a liquid; ii.) forming a slurry containing a liquid and silicon dioxide particles; iii.) treating the slurry with ultrasound to obtain a precursor suspension; iv.) passing at least a portion / preferably the entire precursor suspension through at least a first multi-stage filter device to obtain a silicon dioxide suspension; v.) forming silicon dioxide granules from the silicon dioxide suspension, for example by spray granulation or rotary granulation; vi.) forming a glass melt from the silicon dioxide granules in a furnace; vii.) forming a quartz glass body from at least a portion of the glass melt; The process steps include Treating the slurry in step iii.) includes deagglomerating at least a portion of the silicon dioxide particles; Step v.) comprises granulation, The silicon dioxide granules have a particle size larger than the silicon dioxide particles contained in the silicon dioxide suspension, The furnace has a crucible and a gas outlet; Gas is removed from the furnace via a gas outlet, The dew point of the gas leaving the furnace through the gas outlet is less than 0°C; the first multi-stage filter device has at least first, second and third filter stages, the second filter stage being disposed downstream of the first filter stage and the third filter stage being disposed downstream of the second filter stage; Each filter stage includes at least one filter; the first filter stage has a filter fineness of 5 μm or more, the second filter stage has a filter fineness in the range of 0.5 to 5 μm, and the third filter stage has a filter fineness of 1 μm or less; Filter fineness indicates the smallest particle size that the filter will retain; The separation rate for the first filter stage, in each case calculated in accordance with ISO 16889, is greater than or equal to 50%, for the second filter stage is greater than or equal to 95% and for the third filter stage is greater than or equal to 99.5%.
[0142] Silicon dioxide particle powder In step i.), powder is produced from silicon dioxide particles. Powder of silicon dioxide particles is also called silicon dioxide particle powder. Using the present invention, it is possible in principle to obtain silicon dioxide powder from naturally occurring silicon dioxide or synthetic silicon dioxide, preferably synthetic silicon dioxide powder. It is particularly preferred to use pyrogenically produced silicon dioxide powder.
[0143] The silicon dioxide powder may be any silicon dioxide powder having at least two particles. The manufacturing method may be any method that a person skilled in the art considers to be generally available and suitable for this purpose.
[0144] According to one embodiment of the present invention, silicon dioxide powder is produced as a by-product when producing quartz glass, in particular when producing the so-called "soot body". The silicon dioxide thus produced is often also called "soot dust".
[0145] A suitable source of silicon dioxide powder is silicon dioxide particles obtained when a synthetic soot body is produced using flame hydrolysis burners. When producing the soot body, a rotating carrier tube with a cylindrical jacket surface is moved back and forth along a row of burners. Oxygen and hydrogen can be added here to the flame hydrolysis burners and the initial material to produce primary silicon dioxide particles. The primary silicon dioxide particles preferably have a primary particle size of up to 100 nm. The primary silicon dioxide particles obtained by flame hydrolysis aggregate or agglomerate to form silicon dioxide particles with a particle size of about 9 μm (DIN ISO 13320:2009-1). In the silicon dioxide particles, the primary silicon dioxide particles can be recognized and the primary particle size can be determined by using a scanning electron microscope. A part of the silicon dioxide particles is separated on the cylindrical jacket surface of a carrier pipe rotating about its longitudinal axis, building up the soot body layer by layer. Another fraction of silicon dioxide particles is not separated on the cylindrical jacket surface of carrier pipe, but occurs as dust, for example, in filter system.This other fraction of silicon dioxide particles forms silicon dioxide powder, which is often also called "soot dust".As a rule, the fraction of silicon dioxide particles that separates on carrier pipe is greater than the fraction of silicon dioxide particles that occurs in the process of making soot body, based on the total weight of silicon dioxide particles.
[0146] Today, soot dust is either disposed of as waste with great effort and cost or used without adding value, for example as a filler in road construction, as an additive in the dyeing industry, as a raw material in making tiles and as hexafluorosilicic acid used in cleaning building foundations. In the present invention, it is a suitable starting material and can be processed to give high-value products.
[0147] Silicon dioxide produced by flame hydrolysis is commonly referred to as pyrogenic silicon dioxide. Pyrogenic silicon dioxide is typically available in the form of amorphous primary silicon dioxide particles or silicon dioxide particles.
[0148] According to one embodiment, the silicon dioxide powder can be produced by flame hydrolysis from a gas mixture.In this case, the silicon dioxide particles are also formed in the flame hydrolysis and separated as silicon dioxide powder before any agglomerates or aggregates are formed.The main product here is the silicon dioxide powder referred to as soot dust described above.
[0149] The raw materials for preparing the silicon dioxide powder are preferably organic or inorganic silicon compounds. Non-halogenated silicon compounds are also preferred. Among the organosilicon compounds, compounds in which the silicon atom is directly bonded to an oxygen atom are particularly preferred, in particular siloxanes and silicon alkoxides. "Siloxane" is understood to mean linear and cyclic polyalkylsiloxanes. Polyalkylsiloxanes are preferably represented by the general formula: S p O p R 2p (wherein p is an integer of at least 2, preferably 2 to 10, particularly preferably 3 to 5, and R is an alkyl group having 1 to 8 C atoms, preferably 1 to 4 C atoms, particularly preferably a methyl group).
[0150] Particularly preferred are siloxanes selected from the group consisting of hexamethyldisiloxane, hexamethylcyclotrisiloxane (D3), octamethylcyclotetrasiloxane (D4) and decamethylcyclopentasiloxane (D5) or a combination of two or more thereof. If the siloxane comprises D3, D4 and D5, D4 is preferably the main component. The main component preferably accounts for at least 70% by weight, preferably at least 80% by weight, for example at least 90% by weight or at least 94% by weight, particularly preferably at least 98% by weight, in each case based on the total amount of silicon dioxide powder. Preferred silicon alkoxides are tetramethoxysilane and methyltrimethoxysilane.
[0151] Suitable inorganic silicon compounds as input materials for silicon dioxide powder are silicon halides, silicates, silicon carbide and silicon nitride.Particularly preferred inorganic silicon compounds as input materials for silicon dioxide powder are silicon tetrachloride and trichlorosilane.
[0152] According to one embodiment, the silicon dioxide powder can be made by selecting from the group including siloxanes and silicon alkoxides.
[0153] The silicon dioxide powder is preferably made from a compound selected from the group consisting of hexamethyldisiloxane, hexamethylcyclotrisiloxane, octamethylcyclotetrasiloxane and decamethylcyclopentasiloxane, tetramethoxysilane and methyltrimethoxysilane or a combination of two or more thereof, particularly preferably from octamethylcyclotetrasiloxane.
[0154] When producing silicon dioxide from silicon tetrachloride by flame hydrolysis, various parameters are important. A preferred composition of a suitable gas mixture contains a proportion of oxygen in the flame hydrolysis in the range of 25-40% by volume. The proportion of hydrogen may be in the range of 45-60% by volume. The proportion of silicon tetrachloride is preferably 5-30% by volume, all the above figures in volume percent being based on the total volume of the gas stream. Also preferred are combinations of the above volumetric components for oxygen, hydrogen and SiCl4. The flame in the flame hydrolysis is preferably at a temperature in the range of 1500-2500°C, for example in the range of 1600-2400°C, particularly preferably in the range of 1700-2300°C. The primary silicon dioxide particles formed in the flame hydrolysis are preferably separated as silicon dioxide powder before any agglomerates or aggregates are formed.
[0155] The silicon dioxide powder may have at least one, for example at least two or at least three or at least four, preferably at least five, of the following characteristics: a.35m 2 / g or less, e.g. 25-35m 2 / g, or 20~35m 2 / g, or 25-30m 2 / g range of BET surface area; and b.0.01~0.3g / cm 3 , for example 0.02~0.2g / cm 3 in the range of 0.03 to 0.15 g / cm 3 and more preferably 0.1 to 0.2 g / cm 3 or 0.05 to 0.1 g / cm 3 Bulk density in the range of; c. a carbon content of less than 100 ppm, for example less than 50 ppm or less than 30 ppm, particularly preferably in the range of 1 ppb to 20 ppm; d. a chlorine content of less than 500 ppm, for example less than 300 ppm or less than 150 ppm, particularly in the range of 1 ppb to 80 ppm; e. an aluminum content of less than 200 ppb, for example in the range of 1 to 100 ppb, particularly preferably in the range of 1 to 80 ppb; f. The total content of atoms other than Si, O, H, C, and Cl is less than 5 ppm, for example less than 2 ppm, particularly preferably in the range of 1 ppb to 1 ppm; g. at least 70% by weight of the powder particles have a primary particle size in the range of 10 to 100 nm, for example in the range of 15 to less than 100 nm, particularly preferably in the range of 20 to less than 100 nm; h.0.001~0.3g / cm 3 range, e.g. 0.002~0.2g / cm 3 or 0.005~0.1g / cm 3 in the range of 0.01 to 0.06 g / cm 3 and preferably 0.1 to 0.2 g / cm 3 or 0.15 to 0.2 g / cm 3 Tap density in the range of; i. Residual moisture of less than 5% by weight, for example in the range of 0.25 to 3% by weight, particularly preferably in the range of 0.5 to 2% by weight; j. Particle size distribution D in the range of 1 to 7 μm, for example in the range of 2 to 6 μm or in the range of 3 to 5 μm, particularly preferably in the range of 3.5 to 4.5 μm 10 ; k. Particle size distribution D in the range of 6 to 15 μm, for example in the range of 7 to 13 μm or in the range of 8 to 11 μm, particularly preferably in the range of 8.5 to 10.5 μm 50 ; l. Particle size distribution D in the range of 10 to 40 μm, for example in the range of 15 to 35 μm, particularly preferably in the range of 20 to 30 μm 90 ; or a combination of two or more of characteristics a.-l.; Here, weight percent, ppm and ppb are in each case based on the total weight of the silicon dioxide powder.
[0156] The silicon dioxide powder contains silicon dioxide.Preferably, the silicon dioxide powder contains more than 95% by weight, for example more than 98% by weight, or more than 99% by weight or more than 99.9% by weight, based on the total weight of the silicon dioxide powder in each case.Particularly preferably, the silicon dioxide powder contains more than 99.99% by weight of silicon dioxide, based on the total weight of the silicon dioxide powder.
[0157] The silicon dioxide powder preferably has a content of atoms other than Si, O, H, C, Cl of less than 5 ppm, for example less than 2 ppm, particularly preferably less than 1 ppm, in each case based on the total weight of the silicon dioxide powder.However, in many cases, the silicon dioxide powder contains at least 1 ppb of atoms other than Si, O, H, C, Cl.Atoms other than Si, O, H, C, Cl may be present, for example, as elements, ions, or as part of molecules or ions or complexes.
[0158] Based on the number of powder particles, at least 70% of the silicon dioxide powder particles preferably have a primary particle size of less than 100 nm, for example in the range of 10-100 nm or 15-100 nm, particularly preferably 20-100 nm. The primary particle size is determined by scanning electron microscopy (REM) as described in the "Test Methods" section.
[0159] Based on the number of powder particles, at least 75% of the silicon dioxide powder particles preferably have a primary particle size of less than 100 nm, for example in the range of 10 to 100 nm or 15 to 100 nm, particularly preferably in the range of 20 to 100 nm.
[0160] Based on the number of powder particles, at least 80% of the silicon dioxide powder particles preferably have a primary particle size of less than 100 nm, for example in the range of 10 to 100 nm or 15 to 100 nm, particularly preferably in the range of 20 to 100 nm.
[0161] Based on the number of powder particles, at least 85% of the silicon dioxide powder particles preferably have a primary particle size of less than 100 nm, for example in the range of 10 to 100 nm or 15 to 100 nm, particularly preferably in the range of 20 to 100 nm.
[0162] Based on the number of powder particles, at least 90% of the silicon dioxide powder particles preferably have a primary particle size of less than 100 nm, for example in the range of 10 to 100 nm or 15 to 100 nm, particularly preferably in the range of 20 to 100 nm.
[0163] Based on the number of powder particles, at least 95% of the silicon dioxide powder particles preferably have a primary particle size of less than 100 nm, for example in the range of 10 to 100 nm or 15 to 100 nm, in particular in the range of 20 to 100 nm.
[0164] The silicon dioxide powder is preferably 20 to 35 m 2 / g, e.g. 25~35m 2 / g, or 25-30m 2 / g, the BET surface area being calculated in accordance with DIN 66132 by the Brunauer, Emmet and Teller (BET) method based on the gas absorption at the measured surface area.
[0165] The silicon dioxide powder preferably has a pH value of less than 7, for example in the range of 3 to 6.5 or 3.5 to 6 or 4 to 5.5, particularly preferably in the range of 4.5 to 5. The pH value can be determined by a single rod measuring electrode (4% silicon dioxide powder in water).
[0166] The silicon dioxide powder preferably has a combination of properties a. / b. / c. or a. / b. / f. or a. / b. / g., more preferably a combination of properties a. / b. / c. / f. or a. / b. / c. / g. or a. / b. / f. / g., particularly preferably a combination of properties a. / b. / c. / f. / g.
[0167] The silicon dioxide powder preferably has a combination of properties a. / b. / c. and a BET surface area of 20 to 35 m 2 / g range, bulk density is in the range of 0.05-0.3 g / ml, and carbon content is less than 35 ppm.
[0168] The silicon dioxide powder preferably has a combination of properties a. / b. / f. and a BET surface area of 20 to 35 m 2 / g, the bulk density is in the range of 0.05-0.3 g / ml, and the total content of metals other than aluminum is in the range of 1 ppb-1 ppm.
[0169] The silicon dioxide powder preferably has a combination of properties a. / b. / g. and a BET surface area of 20 to 35 m 2 / g, the bulk density is in the range of 0.05 to 0.3 g / ml, and at least 70% by weight of the powder particles have a primary particle size in the range of 20 to less than 100 nm.
[0170] The silicon dioxide powder more preferably has a combination of properties a. / b. / c. / f. and a BET surface area of 20 to 35 m 2 / g range, bulk density is in the range of 0.05-0.3 g / ml, carbon content is less than 40 ppm, and total content of metals other than aluminum is in the range of 1 ppb-1 ppm.
[0171] The silicon dioxide powder more preferably has a combination of properties a. / b. / c. / g. and a BET surface area of 20 to 35 m 2 / g, the bulk density is in the range of 0.05-0.3 g / ml, the carbon content is less than 40 ppm, and at least 70% by weight of the powder particles have a primary particle size in the range of 20-less than 100 nm.
[0172] The silicon dioxide powder more preferably has a combination of properties a. / b. / f. / g. and a BET surface area of 20 to 35 m 2 / g, the bulk density is in the range of 0.05 to 0.3 g / ml, the total content of metals other than aluminum is in the range of 1 ppb to 1 ppm, and at least 70% by weight of the powder particles have a primary particle size in the range of 20 to less than 100 nm.
[0173] The silicon dioxide powder particularly preferably has a combination of properties a. / b. / c. / f. / g. and a BET surface area of 20 to 35 m 2 / g range, bulk density in the range of 0.05-0.3 g / ml, carbon content less than 40 ppm, total content of metals other than aluminum in the range of 1 ppb-1 ppm, and at least 70% by weight of the powder particles have a primary particle size in the range of 20-100 nm or less.
[0174] Steps i.) to iv.) of the first aspect of the present invention can be understood as follows: i.) providing a powder of silicon dioxide particles and providing a liquid; ii.) forming a slurry containing a liquid and silicon dioxide particles; iii.) treating the slurry with ultrasound to obtain a precursor suspension; iv.) passing at least a portion of the precursor suspension through at least a first multi-stage filter device; the first multi-stage filter device has at least first, second and third filter stages; Each filter stage includes at least one filter; a second filter stage disposed downstream of the first filter stage, and a third filter stage disposed downstream of the second filter stage; the first filter stage has a filter fineness of 5 μm or greater; The second filter stage has a filter fineness of 0.5 to 5 μm, the third filter stage has a filter fineness of 1 μm or less; the separation rate of the first filter stage is 50% or more, the separation rate of the second filter stage is 95% or more and the separation rate of the third filter stage is 99.5% or more, in each case determined in accordance with ISO 16889 and on the basis of the filter; Filter fineness indicates the smallest particle size that the filter will retain.
[0175] Further filter stages may be provided between the first, second and third filter stages.
[0176] For the purposes of the present invention, liquid is taken to mean a substance or mixture of substances that is liquid at a pressure of 1013 hPa and a temperature of 20°C.
[0177] For the purposes of the present invention, "slurry" means a mixture of at least two substances, where under the conditions considered here, the mixture has at least one liquid and at least one solid. During the process, a slurry and a precursor suspension are formed. The precursor suspension is also a slurry, but this one has been treated with ultrasound as described in step iii.). Insofar as the term "slurry" or "precursor suspension" is used below, i.e., insofar as the term "slurry" is used generally, what is described can apply to the slurry, the precursor suspension, or both the slurry and the precursor suspension. This can be justified because, when treating the slurry with ultrasound to obtain the precursor suspension, the treatment does not change all of the properties described below, or, if the properties change, they remain within the properties as generally described.
[0178] Suitable liquids are in principle all substances and mixtures of substances known to those skilled in the art and suitable for this purpose.Preferred liquids are selected from the group comprising organic liquids and water.Silicon dioxide powder in liquid is preferably soluble in an amount of less than 0.5 g / l, preferably less than 0.25 g / l, particularly preferably less than 0.1 g / l, where g / l is expressed as g of silicon dioxide powder per liter of liquid.
[0179] As liquids, preferably polar solutions are suitable. They can be organic liquids or water. The liquid is preferably selected from the group consisting of water, methanol, ethanol, n-propanol, isopropanol, n-butanol, tert-butanol and mixtures of two or more thereof. Water is particularly preferred as liquid. Particularly preferred liquids include distilled or deionized water, for example "maximum purity" water with a conductivity of <0.2 μS / cm.
[0180] The powder is preferably formed from silicon dioxide particles and a liquid slurry. The silicon dioxide particles are almost insoluble in the liquid at room temperature, but may be added to the liquid in a high weight ratio while maintaining a slurry. The slurry is obtained by mixing the components.
[0181] The silicon dioxide particle powder and the liquid can be mixed in any desired manner. For example, the powder can be added to the liquid or the liquid can be added to the powder. The mixture can be stirred during or after the addition. Particularly preferably, the mixture is stirred during and after the addition. The term "stirring" includes shaking and stirring or a combination of both. The powder can be added to the liquid, preferably while stirring the liquid. It is also preferred to add a part of the powder to the liquid, stir the mixture thus obtained, and then mix the mixture with the rest of the powder. Also, a part of the liquid can be added to the powder, stir the mixture thus obtained, and then mix with the rest of the liquid.
[0182] Mixing the silicon dioxide powder with the liquid results in a slurry. The slurry is preferably a suspension in which the silicon dioxide particles are uniformly distributed in the liquid. The term "uniformly" is interpreted to mean that the density and composition of the slurry at any time does not vary by more than 10% from the average density and average composition, in each case based on the total amount of the slurry. As mentioned above, the uniform distribution of the silicon dioxide particles in the liquid can be obtained or maintained by stirring them as described above, or both. The precursor suspension is also a suspension with the above characteristics.
[0183] The slurry and precursor suspension preferably have a weight in the range of 1000-2000 g / l, for example in the range of 1200-1900 g / l or 1300-1800 g / l, particularly preferably in the range of 1400-1700 g / l. The liter weight is determined by weighing a calibrated volumetric container.
[0184] According to one embodiment, the slurry has at least one, for example at least two or at least three or at least four, particularly preferably at least five, of the following properties: A.) the slurry has a solids content of at least 20% by weight, for example in the range from 20 to 70% by weight, or in the range from 30 to 50% by weight, or in the range from 55 to 75% by weight, particularly preferably in the range from 60 to 70% by weight, in each case based on the total weight of the slurry; B.) the slurry has a pH value in the range of 3 or greater, such as greater than 4, or in the range of 4.5 to 8 or 4.5 to 7, where the pH value is determined using a 4 wt.% slurry; C.) In a 4 wt.% slurry, at least 90% of the silicon dioxide particles in the slurry have a particle size according to DIN ISO 13320-1 in the range of 1 nm to <100 μm, for example in the range of 200 to 700 nm; D.) Chlorine content of 500 ppm or less; E.) Content of atoms other than Si, O, H, C, Cl not exceeding 5 ppm; F.) The slurry is rheopectic; G.) The slurry is conveyed in contact with a plastic surface; H.) The slurry is sheared; I.) The slurry has a temperature above 0°C, preferably in the range of 5 to 35°C; J.) the slurry has a viscosity according to DIN 53019-1 (5 rpm, 30% by weight) in the range from 500 to 2000 mPas, for example in the range from 600 to 1700 mPas, particularly preferably in the range from 650 to 1350 mPas; K.) In a 4 wt.% slurry, at least 5% of the silicon dioxide particles in the slurry have a particle size according to DIN ISO 13320-1 in the range of >10 μm.
[0185] According to another embodiment, the precursor suspension likewise has at least one, for example at least two or at least three or at least four, particularly preferably at least five, of the above-mentioned properties A) to K.).
[0186] The silicon dioxide particles in the 4 wt.% aqueous slurry, which have not been pretreated by deagglomeration, preferably have a particle size D in the range of 50 to 250 nm, particularly preferably in the range of 100 to 150 nm. 10 The silicon dioxide particles in the 4 wt. % aqueous slurry preferably have a particle size D in the range of 100 to 400 nm, particularly preferably in the range of 200 to 250 nm. 50 The silicon dioxide particles in the 4 wt. % aqueous slurry preferably have a particle size D in the range of 200 to 600 nm, particularly preferably in the range of 350 to 400 nm. 90 The particle size is determined according to DIN ISO 13320-1. The stated particle size D 10 , D 50 Or D 90 Or a combination of two or more thereof may also be applied to the precursor suspension.
[0187] Particle size is understood to mean the size of the particles that accumulate from the primary particles in the silicon dioxide powder to the silicon dioxide particles in the slurry, precursor suspension or silicon dioxide granules. The average particle size is understood to mean the arithmetic mean of all the particle sizes of the described material. 50 The value indicates that 50% of the particles are smaller than the specified value based on the total number of particles. D 10 The value indicates that 10% of the particles are smaller than the specified value based on the total number of particles. D 90 The value indicates that 90% of the particles are smaller than the specified value based on the total number of particles. The particle size is determined by a dynamic image analysis procedure according to ISO 13322-2:2006-11.
[0188] The term "isoelectric point" is understood to mean the pH value at which the zeta potential assumes the value 0. The zeta potential is determined in accordance with ISO 13099-2:2012.
[0189] The pH value of the slurry is preferably set to a value within the above range. For example, a substance such as NaOH or NH3 can be added to the preferably aqueous slurry solution to adjust the pH value, and the slurry can be frequently stirred. The pH values mentioned for the slurry can also be applied to the pH value of the precursor suspension.
[0190] In step iii.) below, the slurry is ultrasonicated to obtain a precursor suspension. This is done to sonicate the solid particles present in the slurry to deagglomerate them as they constantly build up to form larger structures, also known as agglomerates. The term "deagglomeration" refers to the means and processes that dissolve the accumulation of particles in the suspension or slurry, also referred to as structures herein, and help break the particles apart. There are other methods to deagglomerate such structures in the slurry, such as treating the slurry in a ball mill. Here, typically stainless steel balls move through the liquid, generating kinetic energy that, if it finds such balls in the particle structures to which it is applied, deagglomerates them back into particles. Using a ball mill is considered to be disadvantageous when making high purity materials, as the movement of the balls and the contact of the balls themselves or the grinding vessel constantly wears off material from the balls or the grinding vessel. This is usually metallic and the ball mill contaminates the high purity material as it is made so additional washing steps and / or reprocessing of the milled slurry must be used to remove it from the slurry and / or its subsequent products, which can be expensive and / or time consuming.
[0191] For treatment with ultrasound, in principle any method and any ultrasound source can be used that is known to the person skilled in the art and that seems suitable for the present application.
[0192] In this context, ultrasound is a sound with a peak frequency in the range 20-100 kHz. It may also be a single frequency sound or a bandwidth sound. In the latter case, at least 60% of the ultrasound frequencies used in the range are loaded at the peak frequency ±10 Hz.
[0193] In further embodiments, the slurry is treated with ultrasound for at least 10 seconds, such as at least 20 seconds, or at least 40 seconds, or at least 60, 120, 180 or 240 seconds.
[0194] In further embodiments, the slurry is treated with ultrasound for up to 1000 seconds, such as up to 500 seconds, or up to 200 seconds, or up to 100, 50 or 20 seconds.
[0195] In a further embodiment, the slurry is treated with ultrasound for a period in the range of 10 to 1800 seconds, such as 30 to 1000 seconds, or 30 to 600 seconds, or 40 to 300 seconds.
[0196] The power density of the ultrasonic used is obtained by dividing the power consumption of the ultrasonic source by the volume of the slurry. In a further embodiment, the ultrasonic source used is an ultrasonic generator or an agitating ball mill or a combination of both.
[0197] In a further embodiment, the temperature of the slurry while being sonicated ranges from 5 to 45°C, such as from 10 to 40°C, or from 15 to 40°C.
[0198] In a further embodiment, the ultrasonic power density acting on the slurry is less than 600 W / l, such as less than 450 W / l, or about 300 W / l, the power density being based on the volume of the slurry. The power density is usually not less than 100 W / l.
[0199] In one embodiment, the ultrasonic power density is in the range of 400-500 W / l and the treatment is in the range of 10-90 seconds.
[0200] In another embodiment, the ultrasonic power density is in the range of 300 to 400 W / l, and the treatment time is in the range of 90 to 250 seconds.
[0201] In the deagglomerated 4% by weight slurry, preferably at least 90% of the silicon dioxide particles have a particle size in the range of 1 nm to 1 μm, for example in the range of 30 to 600 nm or 100 to 300 nm, according to DIN ISO 13320-1, where the particle size is measured in a silicon dioxide suspension with a 4% by weight solids content.
[0202] In the deagglomerated 4% by weight slurry, preferably less than 1% of the silicon dioxide particles have a particle size of more than 1 μm according to DIN ISO 13320-1, where the particle size is measured in a silicon dioxide suspension with a 4% by weight solids content.
[0203] In step iv.) below, at least a portion of the precursor suspension is passed through a first multi-stage filter device. After passing through the multi-stage filter device, a silicon dioxide suspension is obtained as filtrate. The first multi-stage filter device has at least a first, a second and a third filter stage. The first multi-stage filter device may have further filter stages, such as a fourth filter stage, optionally a fifth filter stage, optionally a sixth filter stage, etc. The filter stages in the multi-stage filter device are arranged in a specific order. They are numbered in the downstream direction. This means that the precursor suspension first flows through the first filter stage, downstream through the second filter stage, and so on. A multi-filter arrangement is also conceivable, in which different amounts of suspension pass more or less simultaneously through filters arranged adjacent to each other. By arranging several filters adjacent to each other in a filter stage, the service life of the filter stage or the throughput through the filter stage, or both, can be increased. Furthermore, further filter stages may be provided between the first and second filter stages or between the second and third filter stages, which will not be further described here.
[0204] Each filter stage includes at least one filter. A single filter may be provided within a filter stage. Multiple filters may be provided. These are typically arranged adjacent to one another. In this case, the multiple filters used typically have the same characteristic data. Multiple filters may be provided adjacent to one another to divide the flow within the filter stage, as described above, which often increases the useful life or throughput of the filter stage, or both.
[0205] The first filter stage has a filter fineness of 5 μm or more, for example between 5 μm and 15 μm, or about 10 μm, or about 15 μm.
[0206] The second filter stage has a filter fineness in the range of 0.5 to 5 μm, for example in the range of 0.5 to 2 μm, or about 1 μm, or about 2 μm. The third filter stage has a filter fineness of 1 μm or less, for example 1 μm or 0.5 μm.
[0207] At least one filter stage selected from the first, second and third filter stages has a separation efficiency of 99.5% or greater, such as, for example, 99.8% or 99.9%.
[0208] Filter fineness refers to the smallest particle size that a filter with a given effectiveness can filter out, hereinafter also referred to as "x".
[0209] Separation rate or filtration rate ε x In both cases, the standard is ISO 16889:2008. x The value is N x and N h is determined as the quotient of N x is the number of particles upstream of the filter, and N h = the number of particles downstream of the filter, and x is the filter fineness. The filter fineness is the particle size in μm at which the separation rate is determined. Therefore, the separation rate or ε x is (β x -1) / β x It is.
[0210] For example, for a suspension of 400 particles, a 75% separation rate ε 10 means that when the suspension has a particle size of 10 μm or more per unit volume downstream of the filter, 1 out of 100 particles has a particle size of 10 μm or more per unit volume downstream of the filter. In this example, 75% of the particles removed from the suspension had a particle size of 10 μm or more.
[0211] By analogy with the definitions of separation ratio and filter fineness of individual filters, corresponding data for a filter stage comprising one or more individual filters can be obtained using the ranges and preferred embodiments described above.
[0212] The first filter device may have at least one, or two or more, or all of the following characteristics: (a) the first filter stage has a separation efficiency of 90% or less, e.g., 85%, 80%, or 75%, or between 80 and 99.9%, or between 80 and 95%; (b) the first filter stage has a filter fineness of 5 μm or more, in the range of 5 to 25 μm, or 5 to 15 μm, for example 10 μm or 5 μm; (c) the second filter stage has a separation efficiency of 80% or more, such as 95% or more, such as 98%, 99%, 99.9% or 99.99%, or in the range of 80-99.9% or 80-95%; (d) the second filter stage has a filter fineness of 0.5 μm or more, e.g., in the range of 0.5 to 10 μm, or 0.5 to 2 μm, e.g., 0.5 μm, 1.0 μm, 1.5 μm or 2.0 μm; (e) the third filter stage has a separation efficiency of 80% or more, e.g. 99.5% or more, e.g. 99.9% or 99,99%, or in the range of 80-99.9%, or in the range of 95-99.9%; (f) the first filter stage has a filter fineness in the range of 0.5 μm or more, for example in the range of 0.5 to 10 μm, or 0.5 to 3 μm, or 0.5 to 1 μm; Or a combination of two or more of the characteristics (a)-(f) is preferred, with any combination of the values given as examples. In one embodiment, a combination of all the characteristics (a)-(f) is advantageous, for example F1.3 in Table A below.
[0213] In a preferred embodiment, the first filter stage has a filter fineness of 5 μm or more, for example between 5 μm and 25 μm, and a separation efficiency in the range of 80% to 99.9%, preferably between 80% and 95%.
[0214] In a further embodiment, the second filter stage has a filter fineness of 0.5 μm or more, for example in the range of 0.5 μm to 10 μm, and a separation efficiency in the range of 80% to 99.9%, preferably 80% to 95%, preferably 95% to 99.9%.
[0215] In a further embodiment, the third filter stage has a filter fineness of 0.5 μm or more, for example in the range of 0.5 μm to 10 μm, and a separation efficiency in the range of 80% to 99.9%, preferably 95% to 99.9%.
[0216] By way of further example, for example, the first filter device may be characterized by the following combination of properties:
[0217] [Table 1]
[0218] In a further embodiment, the first multi-stage filter device comprises at least one depth filter. In this context, the term "depth filter" is taken to mean a filter in which the particles to be separated are retained over a section in the filter, and a filter cake is not usually formed when the filter is operated. On the other hand, in an area filter or a surface filter, the particles to be separated are separated at the boundary of the surface filter, and a filter cake is formed when the filter is operated. The first multi-stage filter device may also comprise a plurality of depth filters. It is also possible that all filters used in the first multi-stage filter device are depth filters.
[0219] In a further embodiment, at least one further, preferably multi-stage filter device is used downstream of the first multi-stage filter device, and a series of 2, 3, 4, 5, or up to 10 or more downstream multi-stage filter devices arranged in series are provided.
[0220] In a further embodiment, at least a second multi-stage filter device is provided with a depth filter.
[0221] In a further embodiment, the second filter stage of the first filter device comprises at least one first filter having a separation ratio of 90% or less and at least one further filter having a separation ratio of 95% or more.
[0222] In further embodiments, the first multi-stage filter device has a service life of at least 100 liters, for example 150 liters or more, or 250 liters or more, or 500 liters or more, or 800 liters or more, or 1000 liters or more, where liters are based in each case on the volume of precursor suspension filtered by the first multi-stage filter device.
[0223] In further embodiments, the second, optionally multi-stage filter device has a service life of at least 100 liters, for example 150 liters or more, or 250 liters or more, or 500 liters, where liters are based on the volume of precursor suspension that the second filter device filters in each case.
[0224] In relation to a filter device, "service life" means the volume of suspension that can pass through the filter device before it becomes clogged. The occurrence of clogging can be recognized by a rise in pressure upstream of the filter of at least 1.5 times the pressure of a new filter used without changing the pump performance. When a filter becomes clogged, the work step must be suspended and the clogged filter or filters must be cleaned or replaced.
[0225] In a further embodiment, the slurry has less than 5 wt. % of additives, less than 2 wt. %, for example 0 wt. % (none), especially stabilizing additives, where the wt. % is based on the total weight of the slurry. Often, the slurry has at least 0.1 wt. %, for example in the range of 0.1-5 wt. %, of additives, where the wt. % is based on the total weight of the slurry. The additive content usually does not change, or in any case changes very little, during the course of filtration. Thus, both the precursor suspension and the resulting silicon dioxide suspension have a content of stabilizing additives as described for the slurry.
[0226] In a further embodiment, the silicon dioxide suspension obtainable by the process has at least one, for example at least two or at least three or at least four, particularly preferably at least five, of the following properties: A. The silicon dioxide suspension is rheopectic under the specified test conditions, meaning a temperature below 45°C and a solids concentration in the range of 20-70% by weight; B. at least 90% of the silicon dioxide particles in the silicon dioxide suspension have a particle size in the range of 1 nm to <10 μm, for example in the range of 1 nm to 1 μm, 30 to 600 nm, or 100 to 300 nm, or 200 to 300 nm, where the particle size is determined in a silicon dioxide suspension with a 4 wt.-% solids content according to DIN ISO 13320-1; C. the silicon dioxide suspension has a pH value in the range of 3 or more, for example more than 4, or in the range of 4.5 to 8 or 4.5 to 7, where the pH value is determined by a 4 wt.% silicon dioxide suspension; D. Chlorine content less than 500 ppm, not more than 350 ppm, or not more than 200 ppm; E. an aluminum content of less than 200 ppb, for example in the range of 1 to 100 ppb, particularly preferably in the range of 1 to 80 ppb; F. Content of atoms other than Si, O, H, C, and Cl of 5 ppm or less; G. the silicon dioxide suspension has a temperature above 0°C, preferably in the range of 5-35°C; H. the silicon dioxide suspension has a viscosity according to DIN 53019-1 (5 rpm, 30% by weight) in the range from 500 to 2000 mPas, for example in the range from 600 to 1700 mPas, particularly preferably in the range from 650 to 1350 mPas; I. less than 1% of the silicon dioxide particles in the silicon dioxide suspension have a particle size of more than 1 μm, where the particle size is determined in a silicon dioxide suspension with a solids content of 4 wt.-% according to DIN ISO 13320-1; Here, weight percent, ppm and ppb are based on the total amount of silicon dioxide particles in the suspension.
[0227] Preparation of silicon dioxide granules Step v.) then forms silicon dioxide granules, in which the silicon dioxide suspension from step iv.) is further processed. In one embodiment, silicon components other than silicon dioxide may be added in this step.
[0228] The silicon dioxide granules have a larger particle size than the silicon dioxide particles present in the silicon dioxide suspension.
[0229] In principle, silicon dioxide granules can be produced by any process known to those skilled in the art that increases particle size.
[0230] The silicon dioxide granules have a larger particle size than the silicon dioxide powder, which in turn has a larger particle size than the silicon dioxide particles in the silicon dioxide suspension.
[0231] The silicon dioxide granules have a particle size larger than that of the silicon dioxide powder. The particle size of the silicon dioxide granules is preferably 500 to 50,000 times larger than that of the silicon dioxide powder, for example, 1,000 to 10,000 times larger, particularly preferably 2,000 to 8,000 times larger.
[0232] At least 90% of the silicon dioxide granules formed in step iv.), for example at least 95% by weight or at least 98% by weight, particularly preferably at least 99% by weight or more, in each case based on the total weight of the silicon dioxide granules, is preferably made from pyrogenic silicon dioxide powder.
[0233] The processing preferably forms silicon dioxide granules having granules, the granules having a spherical morphology. Preferably, the processing also includes spray granulation or rotary granulation.
[0234] Powder is taken to mean a dry solid matter having a primary particle size in the range from 1 to less than 100 nm.
[0235] Silicon dioxide granules can be obtained by granulating silicon dioxide powder. As a rule, silicon dioxide granules are obtained by granulating silicon dioxide powder. 2 / g and a BET surface area of 1.5 g / cm 3 The term "granulation" is understood to mean the conversion of powder particles into granules. In granulation, agglomerates of multiple silicon dioxide particles, i.e. larger agglomerates called "silicon dioxide granules", are formed. These are also often called "silicon dioxide granule particles" or "granule particles". The granules form a granule as a whole, for example, silicon dioxide granules form "silicon dioxide granules". Silicon dioxide granules have a larger particle size than silicon dioxide powder.
[0236] The granulation process for converting the powder into a granule is described in more detail below.
[0237] In the present context, the term silicon dioxide granules is understood to mean silicon dioxide particles that can be obtained by crushing a silicon dioxide body, in particular a quartz glass body. The silicon dioxide granules usually have a density of 1.2 g / cm 3 Ultra, for example 1.2-2.2g / cm 3 and particularly preferably about 2.2 g / cm 3and the BET surface area of the silicon dioxide granules, when determined according to DIN ISO 9277:2014-01, is usually 2 / g.
[0238] In principle, the silicon dioxide powder may be any and all of those known to those skilled in the art to be suitable, in particular the silicon dioxide particles described in connection with step i.).
[0239] The term "particle diameter" or "particle size" is defined by the formula
[0240]
number
[0241] The granules of the silicon dioxide granules preferably have a spherical morphology. "Spherical morphology" is understood to mean that the particles have a circular to elliptical morphology. The granules of the silicon dioxide granules preferably have an average sphericity in the range of 0.7 to 1.3 SPHT3, for example an average sphericity in the range of 0.8 to 1.2 SPHT3, particularly preferably an average sphericity in the range of 0.85 to 1.1 SPHT3. The properties of SPHT3 are described in the test methods.
[0242] The granules of the silicon dioxide granules also preferably have an average symmetry in the range of 0.7 to 1.3 Symm3, for example an average symmetry in the range of 0.8 to 1.2 Symm3, particularly preferably an average symmetry in the range of 0.85 to 1.1 Symm3. The average symmetry characteristic Symm3 is described in the test method.
[0243] Granulation Silicon dioxide granules are obtained by granulating silicon dioxide powder. The term "granulation" is understood to mean the conversion of powder particles into granules. In granulation, a number of silicon dioxide particles are aggregated to form larger aggregates called "silicon dioxide granules". These are also often called "silicon dioxide granule particles" or "granule particles". The granules as a whole form granules, for example silicon dioxide granules form "silicon dioxide granules".
[0244] In this case, in principle, any granulation method known to those skilled in the art and deemed suitable for granulating silicon dioxide powder can be selected.Granulation methods can be divided into agglomeration granulation and pressure granulation, and further into wet granulation and dry granulation.Known methods are rotary granulation on granulating metal sheet, spray granulation, centrifugal spray, floating bed granulation, freeze granulation and granulation using granulation mill, compression, roller pressing, briquetting, flaking and extrusion.
[0245] Preferably, during processing, the silicon dioxide granules are formed with granules having a spherical morphology, in which case the processing is also preferably by spray granulation or rotary granulation.More preferably, the silicon dioxide granules with granules having a spherical morphology also have granules not having a spherical morphology of less than 50%, preferably less than 40%, also preferably less than 20%, more preferably 0-50%, 0-40% or 0-20%, or 10-50%, 10-40% or 10-20%, the stated percentages being in each case based on the total number of granules in the granules.The granules having a spherical morphology have the SPHT3 value already mentioned in these specifications.
[0246] spray granulation According to a preferred embodiment of step v.), the silicon dioxide granules are formed by spray granulation of the silicon dioxide suspension. Spray granulation is also called spray drying.
[0247] Spray drying is preferably carried out in a spray tower. In spray drying, the silicon dioxide suspension is pressurized at high temperature. The pressurized silicon dioxide suspension is then depressurized through a nozzle and sprayed into a spray tower. Then droplets are formed, which dry instantly and first form dry microparticles ("microbes"). The gas flow acting on the microparticles and particles forms a fluidized bed, so that they can be kept in suspension and form a surface for drying further droplets.
[0248] The nozzle through which the silicon dioxide suspension is sprayed into the spray tower preferably forms an inlet into the interior of the spray tower.
[0249] When spraying, the nozzle preferably has a contact surface with the silicon dioxide suspension.The term "contact surface" is understood to mean the surface of the nozzle that contacts with the silicon dioxide suspension when the suspension is sprayed.In many cases, at least a part of the nozzle is formed as a tube through which the silicon dioxide suspension passes when spraying, so that the inside of the hollow tube contacts with the silicon dioxide suspension.
[0250] The contact surface preferably comprises glass, plastic or a combination thereof. The contact surface preferably comprises glass, particularly preferably quartz glass. The contact surface preferably comprises plastic. In principle, all suitable plastics known to the skilled artisan are those that are stable at the process temperature and do not release any foreign atoms into the silicon dioxide suspension. Preferred plastics are polyolefins, for example homopolymers or copolymers comprising at least one olefin, particularly preferably homopolymers or copolymers comprising polypropylene, polyethylene, polybutadiene or a combination of two or more thereof. Preferably, the contact surface comprises glass, plastic or a combination thereof, for example selected from the group comprising quartz glass and polyolefins, particularly preferably selected from the group comprising quartz glass and homopolymers or copolymers comprising polypropylene, polyethylene, polybutadiene or a combination of two or more thereof. Preferably, the contact surface does not comprise any metal, in particular does not comprise tungsten, titanium, tantalum, chromium, cobalt, nickel, iron, vanadium, zirconium or manganese.
[0251] In principle, the contact surface and the other parts of the nozzle can consist of the same or different materials. Preferably, the other parts of the nozzle comprise the same material as the contact surface. It is also possible that the other parts of the nozzle comprise different materials. For example, the contact surface may be coated with a suitable material, for example glass or plastic.
[0252] Based on the total weight of the nozzle, more than 70% by weight, for example more than 75% by weight, or more than 80% by weight, or more than 85% by weight, or more than 90% by weight, or more than 95% by weight, particularly preferably more than 99% by weight, of the nozzle is formed from an element selected from the group consisting of glass, plastic, or a combination of glass and plastic.
[0253] Preferably, the nozzle comprises a nozzle sheet metal piece. The nozzle sheet metal piece is preferably made of glass, plastic or a combination of glass and plastic. Preferably, the nozzle sheet metal piece is formed of glass, preferably quartz glass. Preferably, the nozzle sheet metal piece is formed of plastic. Preferred plastics are polyolefins, for example homopolymers or copolymers comprising at least one olefin, particularly preferably homopolymers or copolymers comprising polypropylene, polyethylene, polybutadiene or a combination of two or more thereof. Preferably, the nozzle sheet metal piece does not contain any metal, in particular tungsten, titanium, tantalum, chromium, cobalt, nickel, iron, vanadium, zirconium or manganese.
[0254] Preferably, the nozzle comprises a screw twister. The screw twister is preferably made of glass, plastic or a combination of glass and plastic. The screw twister is preferably made of glass, particularly preferably quartz glass. The screw twister is preferably made of plastic. Preferred plastics are polyolefins, for example homopolymers or copolymers comprising at least one olefin, particularly preferably homopolymers or copolymers comprising polypropylene, polyethylene, polybutadiene or a combination of two or more thereof. Preferably, the nozzle metal sheet piece does not contain any metal, in particular tungsten, titanium, tantalum, chromium, cobalt, nickel, iron, vanadium, zirconium or manganese.
[0255] The nozzle can also include further components. Another preferred component is the nozzle body, particularly preferably comprising the screw twister, the nozzle body surrounding the nozzle sheet metal piece, the crosspiece and the impact metal sheet. The nozzle preferably comprises one or more, particularly preferably all, further components. The further components may, independently of one another, in principle comprise any further material known to the skilled person suitable for this purpose, for example metal-based materials, glass or plastic. The nozzle body is preferably formed from glass, particularly preferably from quartz glass. The further components are preferably made of plastic. Preferred plastics are polyolefins, for example homopolymers or copolymers comprising at least one olefin, particularly preferably homopolymers or copolymers comprising polypropylene, polyethylene, polybutadiene or a combination of two or more thereof. Preferably, the nozzle sheet metal piece does not contain any metal, in particular tungsten, titanium, tantalum, chromium, cobalt, nickel, iron, vanadium, zirconium or manganese.
[0256] The spray tower preferably has a gas inlet and a gas outlet. The gas inlet can be used to inject gas into the interior of the spray tower, and the gas can be discharged through the gas outlet. It is also possible to inject gas into the spray tower through a nozzle. Similarly, the gas can be taken out through the spray tower outlet. More preferably, the gas can be supplied to the spray tower through the nozzle and the gas inlet, and taken out of the spray tower through the gas outlet.
[0257] The atmosphere inside the spray tower is preferably air, an inert gas, at least two inert gases, or a combination of air and at least one inert gas, preferably at least two inert gases. The inert gas is preferably selected from the list consisting of nitrogen, helium, neon, argon, krypton and xenon. The atmosphere inside the spray tower is preferably air, nitrogen or argon, particularly preferably air.
[0258] The atmosphere in the spray tower is also preferably part of the gas flow.The gas flow is preferably introduced into the spray tower through the gas inlet and discharged through the gas outlet.A part of the gas flow can also be introduced through a nozzle and discharged through a solid outlet.The gas flow can obtain further components in the spray tower, and these components can come from the silicon dioxide suspension by spray drying and enter the gas flow.
[0259] The gas stream fed to the spray tower is preferably dry. "Dry gas stream" is understood to mean a gas or gas mixture whose relative humidity is below the condensation point at the temperature set in the spray tower. 100% relative air humidity is 17.5 g / m at 20°C. 3 The gas is preferably preheated to a temperature in the range of 150 to 450°C, for example 200 to 420°C or 300 to 400°C, particularly preferably 320 to 400°C.
[0260] The temperature inside the spray tower can be preferably set to a maximum of 550°C, for example 300-500°C, particularly preferably 320-450°C.
[0261] The gas flow at the gas inlet is preferably at a temperature in the range of 150-450°C, for example 200-420°C or 300-400°C, particularly preferably 320-400°C.
[0262] At the solids outlet, the gas outlet or both locations, the discharged gas stream is preferably at a temperature of less than 170°C, for example between 50 and 150°C, particularly preferably between 100 and 130°C.
[0263] More preferably, the difference between the inlet and outlet temperatures of the gas flow is in the range of 100 to 330°C, for example 150 to 300°C.
[0264] The silicon dioxide granules thus obtained are aggregates of individual particles of silicon dioxide powder. Individual silicon dioxide powder particles can still be detected in the aggregates. The average silicon dioxide particle size is preferably in the range of 10-1000 nm, for example in the range of 20-500 nm or 30-250 nm or 35-200 nm or 40-150 nm, or in particular in the range of 50-100 nm. The average particle size of these particles is determined according to DIN ISO 13320-1.
[0265] Spray drying can be carried out in the presence of an excipient. In principle, any and all substances known to those skilled in the art and deemed suitable for the purposes of the present invention can be used as excipient. Excipients that can be considered are, for example, so-called "binders". Examples of suitable binders are metal oxides such as calcium oxide, metal carbonates such as calcium carbonate, and polysaccharides such as cellulose, cellulose ethers, starch and starch derivatives.
[0266] For the purposes of the present invention, spray drying is preferably carried out without excipients.
[0267] A portion of the silicon dioxide granules is preferably separated before, after, or before and after the silicon dioxide granules are removed from the spray tower. It can be separated by any method known to those skilled in the art that is deemed appropriate, such as screening or sieving.
[0268] The particles of the silicon dioxide granules formed by spray drying, having a particle size of less than 50 μm, for example less than 70 μm, particularly preferably less than 90 μm, are preferably screened before removing the granules from the spray tower. Screening is preferably carried out using a cyclone located in the lower region of the spray tower, particularly preferably above the spray tower outlet.
[0269] The portion of the silicon dioxide granules having a particle size of more than 1000 μm, for example more than 700 μm, particularly preferably more than 500 μm, is preferably sieved by any method known in principle to those skilled in the art and suitable for this purpose, preferably using a vibrating chute, after removal of the silicon dioxide granules from the spray tower.
[0270] According to one embodiment, the spray drying of the silicon dioxide suspension through a nozzle in a spray tower is characterized by at least one, for example two or three, particularly preferably all, of the following properties: a] Spray granulation in a spray tower; b] the silicon dioxide in the nozzle is under a pressure of less than or equal to 40 bar, for example in the range of 1.3 to 20 bar or 1.5 to 18 bar, or 2 to 15 bar or 4 to 13 bar, or particularly preferably in the range of 5 to 12 bar, the stated pressures being absolute pressures (based on p=0 hPa); c] The droplets entering the spray tower have a temperature in the range of 10 to 50 ° C, preferably in the range of 15 to 30 ° C, particularly preferably in the range of 18 to 25 ° C; d] the temperature on the side of the nozzle facing the spray tower is in the range from 100 to 450 ° C, for example in the range from 250 to 440 ° C, particularly preferably from 320 to 430 ° C; e] A silicon dioxide suspension is added to 0.05 to 1 m 3 / h range, e.g. 0.1~0.7m 3 / h or 0.2~0.5m 3 / h, and particularly preferably 0.25 to 0.4 m 3 / h range flows through the nozzle; f] the silicon dioxide suspension has a solids content of at least 40% by weight, for example in the range from 50 to 80% by weight or in the range from 55 to 75% by weight, particularly preferably in the range from 60 to 70% by weight, in each case based on the total weight of the silicon dioxide suspension; g] gas flows into the spray tower in the range of 10-100 kg / min, for example in the range of 20-80 kg / min or 30-70 kg / min, particularly preferably in the range of 40-60 kg / min; h] the gas enters the spray tower at a temperature in the range of 100-450 ° C, for example in the range of 250-440 ° C, particularly preferably 320-430 ° C; i] The gas leaves the spray tower at a temperature below 170°C; j] the gas is selected from the group consisting of air, nitrogen and helium or a combination of two or more thereof, preferably air; k] the granules removed from the spray tower have a residual moisture of less than 5%, for example less than 3% by weight or less than 1% by weight or in the range from 0.01 to 0.5% by weight, particularly preferably in the range from 0.1 to 0.3% by weight, in each case based on the total weight of the silicon dioxide granules obtained by spray drying; l] at least 50 wt.-% of the spray granulation, based on the total weight of silicon dioxide obtained from the spray drying, completes a flight time in the range of 1 to 100 seconds, for example over a period of 10 to 80 seconds, particularly preferably over a period of 25 to 70 seconds; m] at least 50 wt.-% of the spray granulate, based on the total weight of silicon dioxide obtained from the spray drying, completes a flight path of more than 20 m, for example more than 30 m, or more than 50 m, or more than 70 m, or more than 100 m, or more than 150 m, or more than 200 m, or in the range from 20 to 200 m, or from 10 to 150 m, or from 20 to 100 m, particularly preferably in the range from 30 to 80 m; n] the spray tower has a cylindrical shape; o] the spray tower has a height of more than 10 m, for example more than 15 m or more than 20 m or more than 25 m or more than 30 m, or in the range from 10 to 25 m, particularly preferably in the range from 15 to 20 m; p] Screening particles less than 90 μm in size before removing the granulation from the spray tower; q] After removing the granulation from the spray tower, particles with a size of more than 500 μm are filtered out, preferably on a vibrating chute; r] The silicon dioxide suspension droplets emerge from the nozzle at an angle of 30 to 60° to the vertical, particularly preferably at an angle of 45° to the vertical.
[0271] "Vertical" is understood to mean the direction of the gravity vector.
[0272] By flight path is meant the path that the silicon dioxide suspended particles take in the spray tower gas space from the time they leave the nozzle while forming granules until they complete the flight and fall process, which generally ends when the granules hit the floor of the spray tower or hit other granules already on the floor of the spray tower, whichever occurs first.
[0273] The flight time is the time it takes for the granules to travel their flight path in the spray tower. The granules in the spray tower preferably have a helical flight path.
[0274] At least 60% by weight of the spray granules, based on the total weight of the silicon dioxide granules obtained from the spray drying, preferably travels an average flight path of more than 20 m, for example more than 30 m, or more than 50 m, or more than 70 m, or more than 100 m, or more than 150 m, or more than 200 m, or in the range of 20 to 200 m, or 10 to 150 m, or 20 to 100 m, particularly preferably 30 to 80 m.
[0275] At least 70% by weight of the spray granules, based on the total weight of the silicon dioxide granules obtained from the spray drying, preferably travels an average flight path of more than 20 m, for example more than 30 m, or more than 50 m, or more than 70 m, or more than 100 m, or more than 150 m, or more than 200 m, or in the range of 20 to 200 m, or 10 to 150 or 20 to 100 m, in particular 30 to 80 m.
[0276] At least 80% by weight of the spray granules, based on the total weight of the silicon dioxide granules obtained from the spray drying, preferably travels an average flight path of more than 20 m, for example more than 30 m, or more than 50 m, or more than 70 m, or more than 100 m, or more than 200 m, or in the range of 20 to 200 m, or 10 to 150 m, or 20 to 100 m, particularly preferably in the range of 30 to 80 m.
[0277] At least 90% by weight of the spray granules, based on the total weight of the silicon dioxide granules obtained by spray drying, preferably travels an average flight path of more than 20 m, for example more than 30 m, or more than 50 m, or more than 70 m, or more than 100 m, or more than 150 m, or more than 200 m, or in the range of 20 m to 200 m, or 10 m to 150 m, or 20 m to 100 m, particularly preferably in the range of 30 m to 80 m.
[0278] Rotary Granulation According to another preferred embodiment of step v.), the silicon dioxide granules are formed by rotary granulation of the silicon dioxide suspension.
[0279] Rotary granulation is carried out by stirring the silicon dioxide suspension in the presence of gas at an elevated temperature. Rotary granulation is preferably carried out in a stirred vessel equipped with a stirring tool. The stirred vessel preferably rotates in the opposite direction to the stirring tool. Preferably, the stirred vessel also has an inlet through which silicon dioxide can be introduced into the stirred vessel, an outlet through which silicon dioxide granules can be removed, a gas inlet and a gas outlet.
[0280] The silicon dioxide suspension is preferably stirred by a pin-type stirring tool. A pin-type stirring tool is understood to mean a stirring tool with a number of long pins whose axial axis is in each case coaxial with the axis of rotation of the stirring tool. The pins preferably trace coaxial circles around the axis of rotation.
[0281] The silicon dioxide suspension is preferably set to a pH value of less than 7, for example to a pH value in the range from 2 to 6.5, particularly preferably to a pH value in the range from 4 to 6. The pH value is preferably set using an inorganic acid, for example an acid selected from the group consisting of hydrochloric acid, sulfuric acid, nitric acid and phosphoric acid, particularly preferably hydrochloric acid.
[0282] The atmosphere in the stirred vessel is preferably selected from air, an inert gas, at least two inert gases, or a combination of air and at least one inert gas, preferably at least two inert gases. The inert gas is preferably selected from the list consisting of nitrogen, helium, neon, argon, krypton and xenon. For example, the stirred vessel contains air, nitrogen or argon, particularly preferably air.
[0283] The atmosphere in the stirred vessel is also preferably part of the gas flow. The gas flow in the stirred vessel is preferably introduced through a gas inlet and removed through a gas outlet. The gas flow can absorb further components in the stirred vessel, which in the rotary granulation originate from the silicon dioxide suspension and can enter the gas flow.
[0284] A dry gas stream is preferably added to the stirred vessel. "Dry gas stream" is understood to mean a gas or gas mixture whose relative humidity at the set temperature in the stirred vessel is below the dew point. The gas is preferably preheated to a temperature in the range of 50-300°C, for example 80-250°C, particularly preferably 100-200°C.
[0285] Preferably, for every kg of silicon dioxide suspension used, the rate is 10 to 150 m per hour. 3 of gas, e.g. 20-100 m per hour 3 of gas, particularly preferably 30 to 70 m per hour 3 of gas is fed into the stirred vessel.
[0286] The gas stream dries the silicon dioxide suspension while stirring to form silicon dioxide granules. The formed granules are removed from the stirring chamber.
[0287] The removed granules are preferably further dried, preferably continuously, for example in a rotary kiln. The preferred drying temperature is in the range of 80 to 250°C, for example in the range of 100 to 200°C, particularly preferably in the range of 120 to 180°C.
[0288] In the context of the present invention, continuous means a process that can be operated continuously. This means that the substances and materials involved in carrying out the process can be added and removed during operation. There is no need to interrupt the process.
[0289] As an attribute of an object, for example a "continuous furnace," "continuous" means that the process or process steps carried out therein can be carried out continuously.
[0290] The granulate obtained by rotary granulation can be filtered before or after drying. It is preferably filtered before drying. The filtered granulate preferably has a particle size of less than 50 μm, for example less than 80 μm, particularly preferably less than 100 μm. The filtered granulate also has a particle size of more than 900 μm, for example more than 700 μm, particularly preferably more than 500 μm. Larger particles can in principle be filtered out by any and all processes known to those skilled in the art and suitable for this purpose. Larger particles are preferably filtered out by a vibrating chute.
[0291] In a further embodiment, the rotogranulation is characterized by at least one, for example two or three, particularly preferably all, of the following properties: [a] Granulation is carried out in a rotating stirred vessel; [b] the granulation is carried out under a gas flow of 10-150 kg of gas per kg of silicon suspension per hour; [c] The input gas temperature is 40 to 200°C; [d] Particulate matter having a particle size of less than 100 μm and more than 500 μm is filtered out; [e] the formed granules have a residual moisture of 15-30% by weight; [f] The formed granules are dried at 80-250° C., preferably in a continuous drying tube, in particular until the residual moisture is less than 1% by weight.
[0292] The silicon dioxide granules obtained by granulation, in particular spray granulation or rotary granulation, are further pretreated before being processed into a quartz glass body. This pretreatment can serve different purposes, either to facilitate processing into a quartz glass body or to affect the properties of the resulting quartz glass body. For example, the silicon dioxide granules can be compressed, washed, surface modified or dried.
[0293] In the following, the silicon dioxide granules obtained by granulation but which have not been further pretreated and / or have not yet been pretreated are referred to as "silicon dioxide granules I". In the following, the silicon dioxide granules produced according to one or more pretreatment steps before forming the glass melt are referred to as "silicon dioxide II".
[0294] The silicon dioxide granules obtained by granulation, i.e. silicon dioxide granules I, can have at least one, preferably two or more of the following properties: [A] 20~50m 2 / g range, e.g. 20~40m 2 / g, particularly preferably 25 to 35m 2 / g; the microporous component in this case is preferably 4 to 5 m 2 / g range; e.g., 4.1 to 4.9 m 2 / g range; particularly preferably 4.2 to 4.8 m 2 / g range; and [B] an average particle size in the range of 180 to 300 μm, for example, in the range of 220 to 280 μm, particularly preferably in the range of 230 to 270 μm; [C] 0.5~1.2g / cm 3 range, e.g. 0.6~1.1g / cm 3 In particular, the range of 0.7 to 1.0 g / cm 3 Bulk density in the range of; [D] a carbon content of less than 50 ppm, for example less than 40 ppm, or less than 30 ppm, or less than 20 ppm, or less than 10 ppm, particularly preferably in the range of 1 ppb to 5 ppm; [E] an aluminum content of less than 200 ppb, preferably less than 100 ppb, for example less than 50 ppb or in the range of 1 to 200 ppb or 15 to 100 ppb, particularly preferably 1 to 50 ppb; [F] 0.5~1.2g / cm 3 range, e.g. 0.6~1.1g / cm 3 in the range of 0.75 to 1.0 g / cm 3 Tap density in the range of; [G] a pore volume in the range of 0.1 to 1.5 ml / g, for example in the range of 0.15 to 1.1 ml / g, particularly preferably in the range of 0.2 to 0.8 ml / g; [H] a chlorine content of less than 200 ppm, preferably less than 150 ppm, for example less than 100 ppm, or less than 50 ppm, or less than 1 ppm, or less than 500 ppb, or less than 200 ppb, or from 1 ppb to less than 200 ppm, or from 1 ppb to 100 ppm, or from 1 ppb to 1 ppm, or from 10 ppb to 500 ppb, or from 10 ppb to 200 ppb, particularly preferably from 1 ppb to 80 ppb; [I] A metal content of metals other than aluminum of less than 1000 ppb, preferably in the range of 1 to 900 ppb, for example in the range of 1 to 700 ppb, particularly preferably in the range of 1 to 500 ppb; [J] residual moisture of 10% by weight, preferably in the range of 0.01% by weight to 5% by weight, for example 0.02 to 1% by weight, particularly preferably 0.03 to 0.5% by weight; Here, wt.%, ppm and ppb are in each case based on the total weight of silicon dioxide granules I.
[0295] The OH content, or hydroxyl group content, is understood to mean the OH group content of a material, such as a silicon dioxide powder, a silicon dioxide granule or a quartz glass body. The OH group content is determined spectroscopically in the infrared by comparing the first and third OH bands.
[0296] The chlorine content is understood to mean the elemental chlorine or chloride ion content of the silicon dioxide granules, silicon dioxide powder or quartz glass body.
[0297] The term "aluminum content" is understood to mean the elemental aluminum or aluminum ion content of the silicon dioxide granules, silicon dioxide powder or quartz glass body.
[0298] The silicon dioxide granules I are preferably 4 to 5 m 2 / g range, e.g. 4.1-4.9m 2 / g, particularly preferably 4.2 to 4.8 m 2 / g range of micropore content.
[0299] The silicon dioxide granules I preferably have a density of 2.1 to 2.3 g / cm 3 In particular, the range of 2.18 to 2.22 g / cm 3 It has a density in the range of
[0300] Particle size is understood to mean the size of the particles combined from the primary particles in the silicon dioxide powder, in the slurry or in the silicon dioxide granules.
[0301] Average particle size is understood to mean the arithmetic mean of all particle sizes of the material. 50 The value indicates that 50% of the particles are below that value, based on the total number of particles. D 10 The value indicates that 10% of the particles are below that value, based on the total number of particles. D 90 The value indicates that 90% of the particles are below that value based on the total number of particles. Particle size is determined by dynamic image analysis according to ISO 13322-2:2006-11.
[0302] The silicon dioxide granules I preferably have a particle size D in the range of 150 to 300 μm, for example in the range of 180 to 280 μm, particularly preferably in the range of 220 to 270 μm. 50 The silicon dioxide granules also preferably have a particle size D in the range of 50 to 150 μm, for example in the range of 80 to 150 μm, particularly preferably in the range of 100 to 150 μm. 10The silicon dioxide granules also preferably have a particle size D in the range of 250 to 620 μm, for example in the range of 280 to 550 μm, particularly preferably in the range of 300 to 450 μm. 90 has.
[0303] The silicon dioxide granules I preferably have a combination of properties [A] / [B] / [C] or [A] / [B] / [E] or [A] / [B] / [G], more preferably a combination of properties [A] / [B] / [C] / [E] or [A] / [B] / [C] / [G] or [A] / [B] / [E] / [G], particularly preferably a combination of properties [A] / [B] / [C] / [E] / [G].
[0304] The silicon dioxide granules I preferably have a combination of properties [A] / [B] / [C] and a BET surface area of 20 to 40 m 2 / g, the average particle size is in the range of 180 to 300 μm, and the bulk density is in the range of 0.6 to 1.1 g / ml.
[0305] The silicon dioxide granules I preferably have a combination of properties [A] / [B] / [E] and a BET surface area of 20 to 40 m 2 / g, the average particle size is in the range of 180 to 300 μm, and the aluminum content is in the range of 1 to 50 ppb.
[0306] The silicon dioxide granules I preferably have a combination of properties [A] / [B] / [G] and a BET surface area of 20 to 40 m 2 / g, the average particle size is in the range of 180 to 300 μm, and the pore volume is in the range of 0.2 to 0.8 ml / g.
[0307] The silicon dioxide granules I preferably have a combination of properties [A] / [B] / [C] / [E] and a BET surface area of 20 to 40 m 2 / g, average particle size is in the range of 180-300 μm, bulk density is in the range of 0.6-1.1 g / ml, and aluminum content is in the range of 1-50 ppb.
[0308] The silicon dioxide granules I preferably have a combination of properties [A] / [B] / [C] / [G] and a BET surface area of 20 to 40 m 2 / g, average particle size is in the range of 180-300 μm, bulk density is in the range of 0.6-1.1 g / ml, and pore volume is in the range of 0.2-0.8 ml / g.
[0309] The silicon dioxide granules I preferably have a combination of properties [A] / [B] / [E] / [G] and a BET surface area of 20 to 40 m 2 / g, the average particle size is in the range of 180-300 μm, the aluminum content is in the range of 1-50 ppb, and the pore volume is in the range of 0.2-0.8 ml / g.
[0310] The silicon dioxide granules I preferably have a combination of properties [A] / [B] / [C] / [E] / [G] and a BET surface area of 20 to 40 m 2 / g, average particle size is in the range of 180-300 μm, bulk density is in the range of 0.6-1.1 g / ml, aluminum content is in the range of 1-50 ppb, and pore volume is in the range of 0.2-0.8 ml / g.
[0311] Optional processing of granulated materials The silicon dioxide granules I may be subjected to a thermal, mechanical or chemical treatment, or a combination of two or more treatments, to obtain silicon dioxide granules.
[0312] a.Chemical According to a preferred embodiment of the first subject of the present invention, the silicon dioxide granules I have a carbon content w C(1) The carbon content w C(1) is preferably in the range of less than 50 ppm, for example less than 40 ppm or less than 30 ppm, particularly preferably in the range of 1 ppb to 20 ppm, in each case based on the total weight of the silicon dioxide granules.
[0313] According to a preferred embodiment of the first subject of the present invention, the silicon dioxide granules comprise at least two particles. The at least two particles can preferably move relative to each other. This relative movement can in principle be caused by any known suitable means that would be suitable for a person skilled in the art. Mixing is particularly preferred. Mixing can in principle be carried out in any desired manner, preferably using a continuous oven. Correspondingly, the at least two particles can preferably be moved relative to each other by being moved in a continuous oven, for example a rotary oven.
[0314] By continuous oven is meant an oven that is continuously charged and discharged ("loaded"). Examples of continuous ovens are rotary ovens, roll ovens, conveyor belt ovens, continuous ovens and pusher ovens. The silicon dioxide granules I are preferably processed using rotary ovens.
[0315] According to a preferred embodiment of the first subject of the present invention, the silicon dioxide granules are treated with a reagent to obtain silicon dioxide II. The treatment is carried out to change the concentration of certain substances in the silicon dioxide granules. The silicon dioxide granules I may have contaminants or certain functional groups whose proportions should be reduced, such as, for example, OH groups, carbon compounds, transition metals, alkali metals and alkaline earth metals. The contaminants and functional groups may arise in the input material or in the course of the process. The silicon dioxide granules I can serve various purposes, for example, by using the treated silicon dioxide granules I, i.e., silicon dioxide granules II, the processing of the silicon dioxide granules into a quartz glass body can be simplified. This selection can also be used to adapt the properties of the resulting quartz glass body. For example, the silicon dioxide granules I can be washed or surface modified. That is, the silicon dioxide granules I can be used to improve the properties of the resulting quartz glass body.
[0316] Reagents such as gases or combinations of two or more gases are preferably suitable. These are also called gas mixtures. In principle, any and all gases known to those skilled in the art that are known and deemed suitable for the process can be used. Preferably, the gas is selected from the group consisting of HCl, Cl2, F2, O2, O3, H2, C2F4, C2F6, HClO4, air, inert gases such as N2, He, Ne, Ar, Kr, or combinations of two or more thereof. The process is preferably carried out in the presence of one gas or a combination of two or more gases as gas, preferably in gas countercurrent or parallel gas flow.
[0317] The reagent is preferably selected from the group consisting of HCl, Cl 2 , F 2 , O 2 , O 3 or a combination of two or more thereof. A mixture of two or more of the aforementioned gases is preferably used to treat the silicon dioxide granules I.
[0318] The presence of F, Cl or both can remove metals, such as transition metals, alkali metals and alkaline earth metals, contained in the silicon dioxide granules I as contaminants. Here, the above metals can be combined with the components of the gas mixture to give gaseous components under process conditions, which are then removed from the granules and are therefore no longer present in the granules. More preferably, the OH content of the silicon dioxide granules I can be reduced by treating the silicon dioxide granules I with these gases.
[0319] A mixture of HCl gas and Cl2 gas is preferably used as the reagent. Preferably, the gas mixture has an HCl content in the range of 1-30% by volume, for example in the range of 2-15% by volume, particularly preferably in the range of 3-10% by volume. Also preferably, the gas mixture has a Cl2 content in the range of 20-70% by volume, for example in the range of 25-65% by volume, particularly preferably in the range of 30-60% by volume. The remainder of 100% by volume may consist of one or more inert gases, for example N2, He, Ne, Ar, Kr or air. The inert gas component of the reagent is preferably in the range of 0-50% by volume or less, for example in the range of 1-40% by volume or 5-30% by volume, particularly preferably in the range of 10-20% by volume, in each case based on the total volume of the reagent.
[0320] O 2 , C 2 F 2 , or a mixture thereof with Cl 2 is preferably used to purify silicon dioxide granules I made from a siloxane or a mixture of two or more siloxanes.
[0321] The reagent in the form of a gas or gas mixture is preferably contacted with the silicon dioxide granules as a gas stream or part of a gas stream with a throughput in the range of 50 to 2000 l / h, for example in the range of 100 to 1000 l / h, particularly preferably in the range of 200 to 500 l / h. A preferred design of contact is the contact of the gas stream with the silicon dioxide granules in a continuous oven, for example a rotary tube oven. Another preferred form of contact is the fluidized bed process.
[0322] By treating the silicon dioxide granules I with a reagent, the carbon content w C(2) The silicon dioxide granules II having the carbon content w C(2) is less than the carbon content of silicon dioxide granules III and less than the carbon content of silicon dioxide granules I, in each case based on the total weight of the silicon dioxide granules concerned C(1) Preferably, w C(2) , w C(1) is 0.5 to 99%, for example 20 to 80% or 50 to 95%, particularly preferably 60 to 99% less than the above.
[0323] b.Thermal Prior to forming the glass melt, the silicon dioxide granules are preferably also subjected to a thermal or mechanical treatment or a combination of these treatments. One or more of these additional treatments may be used before or during the treatment with the reagent. Alternatively or additionally, additional treatments may be performed on the silicon dioxide granules II. The general term "silicon dioxide granules" used below includes the alternative forms "silicon dioxide granules I" and "silicon dioxide granules II". It is also possible to perform the treatments described below on both "silicon dioxide granules I" and the treated silicon dioxide granules I, "silicon dioxide granules II". Such a heat treatment is preferably used after any of the above-mentioned chemical treatments.
[0324] Processing the silicon dioxide granules can serve various purposes. For example, the processing makes it easier to process the silicon dioxide granules into a quartz glass body. The processing can also affect the properties of the resulting quartz glass body. For example, the silicon dioxide granules may be compressed, washed, surface modified, or dried, which can reduce the specific surface area (BET). Agglomerating the silicon dioxide particles can also increase their bulk density and average particle size. The heat treatment can be dynamic or static.
[0325] In principle, any furnace suitable for dynamic heat treatment is a furnace in which the silicon dioxide granules are heat treated and can be moved during the process. Dynamic heat treatment preferably uses a continuous furnace.
[0326] The preferred average residence time of the silicon dioxide granules in the dynamic heat treatment depends on the amount. In the dynamic heat treatment, the average residence time of the silicon dioxide granules is preferably in the range of 10 to 180 minutes, for example in the range of 20 to 120 minutes or in the range of 30 to 90 minutes. Particularly preferably, when thermodynamically treated, the silicon dioxide granules have an average residence time in the range of 30 to 90 minutes.
[0327] In the case of a continuous process, the residence time of the charge is a defined portion of the flow rate of the silicon dioxide granules, for example, g, kg or t. The residence time here starts when the granules are fed into the continuous furnace operation and ends when the granules are discharged from the continuous furnace operation.
[0328] In the continuous thermodynamic heat treatment process, the throughput of the silicon dioxide granules is preferably in the range of 1 to 50 kg / h, for example in the range of 5 to 40 kg / h or 8 to 30 kg / h. Particularly preferably, the throughput is in the range of 10 to 20 kg / h.
[0329] For discontinuous thermodynamic treatment processes, the treatment time is the time between charging and unloading the furnace.
[0330] In the case of discontinuous dynamic heat treatment processes, the throughput is in the range of 1-50 kg / h, for example in the range of 5-40 kg / h or 8-30 kg / h. Particularly preferably, the throughput is in the range of 10-20 kg / h. The throughput can be achieved by charging a given amount to be treated in one hour. According to another embodiment, the throughput can be achieved by the number of batches per hour, for example the amount of the batch is equal to the throughput per hour divided by the number of batches. The treatment time is then equal to the percentage of one hour obtained by dividing 60 minutes by the number of batches per hour.
[0331] The silicon dioxide granules are preferably dynamically heat treated at an oven temperature of at least 500 ° C, for example in the range of 510 to 1700 ° C or 550 to 1500 ° C or 580 to 1300 ° C, particularly preferably in the range of 600 to 1200 ° C.
[0332] As a general rule, the furnace in the furnace chamber is at a defined temperature, which preferably varies by less than ±10% from the temperature both at any time of the process and anywhere in the furnace, based on the total process time and the total length of the furnace.
[0333] Alternatively, a continuous process of dynamic heat treatment of the silicon dioxide granules may be carried out, in particular at different oven temperatures. For example, over the treatment time, the oven may be at a constant temperature, and the temperature varies from section to section over the length of the oven. Such sections may be of the same or different length. In this case, the temperature preferably increases from the oven inlet to the oven outlet. The temperature at the inlet is preferably at least 100 ° C lower than the temperature at the outlet, for example 150 ° C lower, or 200 ° C lower, or 300 ° C lower, or 400 ° C lower. The temperature at the outlet is also preferably at least 500 ° C, for example in the range of 510-1700 ° C or 550-1500 ° C or 580-1300 ° C, particularly preferably in the range of 600-1200 ° C; the temperature at the inlet is preferably at least 300 ° C, for example 400-1000 ° C or 450-900 ° C or 500-800 ° C or 550-750 ° C, particularly preferably 600-700 ° C. Any of the furnace inlet temperature range conditions can be combined with any of the furnace outlet temperature ranges. Preferred combinations of furnace inlet and outlet temperature ranges are as follows:
[0334] [Table 2]
[0335] The static heat treatment of the silicon dioxide granules is preferably carried out in a crucible placed in a furnace. Suitable crucibles are sintered crucibles or metal sheet crucibles. Roller metal sheet crucibles made of multiple rates riveted together are preferred. The crucible material is, for example, a refractory metal, in particular tungsten, molybdenum and tantalum. The crucible may also be made of graphite or, in the case of a refractory metal furnace, may be punched out of graphite foil. Preferably, the crucible may be made of silicon dioxide. Silicon dioxide crucibles are particularly preferably used.
[0336] The average residence time of the silicon dioxide granules when statically thermally treated depends on the amount. The average residence time of the silicon dioxide granules when statically thermally treated with an amount of 20 kg of silicon dioxide granules I is preferably in the range of 10 to 180 minutes, for example in the range of 20 to 120 minutes, particularly preferably in the range of 30 to 90 minutes.
[0337] The silicon dioxide granules are preferably treated at an oven temperature of at least 800 ° C, for example in the range of 900 to 1700 ° C or 950 to 1600 ° C or 1000 to 1500 ° C or 1050 to 1400 ° C, particularly preferably in the range of 1100 to 1300 ° C.
[0338] The preferably statically heat-treated silicon dioxide granules I are preferably treated at a constant oven temperature. It may also be statically heat-treated at a variable oven temperature, in which case the temperature is preferably decreased during the course of the treatment, the treatment starting at a temperature at least 50 ° C lower than when it ends, for example 70 ° C lower, or 80 ° C lower, or 100 ° C lower, or 110 ° C lower, and the temperature preferably ends at a temperature of at least 800 ° C, for example in the range of 900 to 1700 ° C, or 950 to 1600 ° C, or 1000 to 1500 ° C, or 1050 to 1400 ° C, particularly preferably in the range of 1100 to 1300 ° C.
[0339] c. Mechanical According to a further preferred embodiment, the silicon dioxide granules are mechanically treated before forming the glass melt. By mechanically treating the silicon dioxide granules, it is possible to increase their bulk density. The silicon dioxide granules can be mechanically treated after being thermally treated as described above. By mechanically treating the silicon dioxide granules, it is possible to avoid the agglomerates in the silicon dioxide granules and thus the average particle size of the individual silicon dioxide granules in the silicon dioxide granules becoming too large. Having too large agglomerates can make further processing more difficult or can adversely affect the properties of the quartz glass body produced by the method as in the present invention, or can mean a combination of both effects. Mechanically treating the silicon dioxide granules also promotes uniform contact between the surface of the individual silicon dioxide granules and the gas. In particular, this is achieved by a combination of simultaneous mechanical and chemical treatment with one or more gases, improving the effectiveness of the chemical treatment.
[0340] The silicon dioxide granules can be produced by moving two or more silicon dioxide granules relative to each other, for example by rotating the tubes of a rotary tube furnace.
[0341] The silicon dioxide granules I are preferably treated chemically, thermally and mechanically. The treatments may be used simultaneously, sequentially or overlapping. Overlapping means that one treatment is not completed before the next begins. The criterion for evaluating the time series is what is being done to the charge of silicon dioxide granules, and not, for example, the operating time of the individual processes as a whole. The silicon dioxide granules I are in particular treated chemically, thermally and mechanically simultaneously.
[0342] Chemical treatment reduces the content of contaminants in the silicon dioxide granules I. For this purpose, the silicon dioxide granules I can be treated in a rotary tube furnace at elevated temperature under a chlorine and oxygen atmosphere. This causes the water in the silicon dioxide granules I to evaporate and the organic material to react to CO and CO2. Metal contaminants can be converted into volatile chlorine compounds.
[0343] The silicon dioxide granules I are preferably treated in a rotary kiln in a chlorine and oxygen atmosphere at a temperature of at least 500 ° C, preferably in the temperature range of 550-1300 ° C or 600-1260 ° C or 650-1200 ° C or 700-1000 ° C, particularly preferably in the temperature range of 700-900 ° C. The chlorine-containing atmosphere contains, for example, HCl or Cl2 or a combination of both. This treatment reduces the carbon content.
[0344] Alkali and iron contamination is also preferably reduced, and a reduction in the number of OH groups is also preferably achieved. At temperatures below 700°C, the treatment time may be long, and at temperatures above 1100°C, there is a risk of closing the pores of the granules and trapping chlorine or gaseous chlorine compounds.
[0345] d. Combined treatment Preferably, two or more chemical treatment steps can be carried out in succession with simultaneous thermal and mechanical treatment. For example, the silicon dioxide granules can be treated first in a chlorine atmosphere and then in an oxygen atmosphere. The resulting low concentrations of carbon, hydroxyl groups and chlorine help melt the granules.
[0346] According to a further preferred embodiment, the pretreatment of the silicon dioxide granules before forming the glass melt is characterized by a combination of at least one or at least two or at least three, particularly preferably all, of the following properties: N1) the reagent comprises HCl, Cl2 or a combination thereof; N2) treatment is carried out in a rotary furnace; N3) the treatment is carried out at a temperature in the range of 600-900 ° C; N4) Reagents form a countercurrent flow; N5) the reagent has a gas throughput in the range of 50-2000 l / h, preferably 100-1000 l / h, particularly preferably 200-500 l / h; N6) The reagent contains an inert gas in the range of 0 to less than 50% by volume.
[0347] The silicon dioxide granules thus obtained are, as already mentioned above, also known as silicon dioxide granules II. Particularly preferably, silicon dioxide granules II are obtained from silicon dioxide granules I in a rotary kiln by a combination of thermal, mechanical and chemical treatments.
[0348] The silicon dioxide granules II may have one or more of the following characteristics: (A) 10~35m 2 / g range, e.g. 10~30m 2 / g, particularly preferably 20 to 30m 2 / g range of BET surface area; and (B) an average particle size in the range of 100 to 300 μm, for example, 150 to 280 μm or 200 to 270 μm, particularly preferably 230 to 260 μm; (C) 0.7~1.2g / cm 3 range, e.g. 0.75-1.1g / cm 3 In particular, the range of 0.8 to 1.0 g / cm 3 Bulk density in the range of; (D) a carbon content of less than 5 ppm, for example less than 4.5 ppm or in the range of 1 ppb to 4 ppm, particularly preferably less than 4 ppm; (E) an aluminum content of less than 200 ppb, for example less than 150 ppb or less than 100 ppb or in the range of 1 to 150 ppb or 1 to 100 ppb, particularly preferably in the range of 1 to 80 ppb; (F) 0.7~1.2g / cm 3 range, e.g. 0.75-1.1g / cm 3 In particular, the range of 0.8 to 1.0 g / cm 3 Tap density in the range of; (G) a pore volume in the range of 0.1 to 2.5 ml / g, for example in the range of 0.2 to 1.5 ml / g, particularly preferably in the range of 0.4 to 1 ml / g; (H) a chlorine content of less than 500 ppm, preferably less than 400 ppm, for example less than 350 ppm or preferably less than 330 ppm, or in the range of 1 ppb to 500 ppm or 10 ppb to 450 ppm, particularly preferably 50 ppb to 300 ppm; (I) a metal content of metals other than aluminum of less than 1000 ppb, for example in the range of 1 to 400 ppb, particularly preferably in the range of 1 to 200 ppb; (J) a residual moisture content of less than 3% by weight, for example in the range of 0.001% to 2% by weight, particularly preferably in the range of 0.01 to 1% by weight; Here, wt.%, ppm and ppb are in each case based on the total weight of silicon dioxide granules II.
[0349] The silicon dioxide granules II are preferably 1 to 2 m 2 / g range, e.g. 1.2~1.9m 2 / g, particularly preferably 1.3 to 1.8 m 2 / g range of micropore content.
[0350] The silicon dioxide granules II preferably have a density of 0.5 to 2.0 g / cm 3 , e.g. 0.6~1.5g / cm 3 , particularly preferably 0.8 to 1.2 g / cm 3 The density is determined by the method described in the test methods.
[0351] The silicon dioxide granules II preferably have a particle size D in the range of 150 to 250 μm, for example in the range of 180 to 250 μm, particularly preferably in the range of 200 to 250 μm. 50 Particularly preferably, the silicon dioxide granules II have a particle size D in the range of 50 to 150 μm, for example in the range of 80 to 150 μm, particularly preferably in the range of 100 to 150 μm. 10 More preferably, the silicon dioxide granules II have a particle size D in the range of 250 to 450 μm, for example in the range of 280 to 420 μm, in particular in the range of 300 to 400 μm. 90 has.
[0352] The silicon dioxide granules II preferably have a combination of properties (A) / (B) / (D) or (A) / (B) / (F) or (A) / (B) / (I), more preferably a combination of properties (A) / (B) / (D) / (F) or (A) / (B) / (D) / (I) or (A) / (B) / (F) / (I), particularly preferably a combination of properties (A) / (B) / (D) / (F) / (I).
[0353] The silicon dioxide granules II preferably have a combination of properties (A) / (B) / (D) and a BET surface area of 10 to 30 m 2 / g, the average particle size is in the range of 150 to 280 μm, and the carbon content is less than 4 ppm.
[0354] The silicon dioxide granules II preferably have a combination of properties (A) / (B) / (F) and a BET surface area of 10 to 30 m 2 / g, the average particle size is in the range of 150 to 280 μm, and the tap density is in the range of 0.8 to 1.0 g / ml.
[0355] The silicon dioxide granules II preferably have a combination of properties (A) / (B) / (I) and a BET surface area of 10 to 30 m 2 / g, the average particle size is in the range of 150 to 280 μm, and the metal content of metals other than aluminum is in the range of 1 to 400 ppb.
[0356] The silicon dioxide granules II preferably have a combination of properties (A) / (B) / (D) / (F) and a BET surface area of 10 to 30 m 2 / g, the average particle size is in the range of 150 to 280 μm, the carbon content is less than 4 ppm, and the tap density is in the range of 0.8 to 1.0 g / ml.
[0357] The silicon dioxide granules II preferably have a combination of properties (A) / (B) / (D) / (I) and a BET surface area of 10 to 30 m 2 / g, the average particle size is in the range of 150 to 280 μm, the carbon content is less than 4 ppm, and the metal content of metals other than aluminum is in the range of 1 to 400 ppb.
[0358] The silicon dioxide granules II preferably have a combination of properties (A) / (B) / (F) / (I) and a BET surface area of 10 to 30 m 2 / g, the average particle size is in the range of 150 to 280 μm, the tap density is in the range of 0.8 to 1.0 g / ml, and the metal content of metals other than aluminum is in the range of 1 to 400 ppb.
[0359] The silicon dioxide granules II preferably have a combination of properties (A) / (B) / (D) / (F) / (I) and a BET surface area of 10 to 30 m 2 / g, average particle size is in the range of 150-280 μm, carbon content is less than 4 ppm, tap density is in the range of 0.8-1.0 g / ml, and metal content of metals other than aluminum is in the range of 1-400 ppb.
[0360] The silicon dioxide granules (silicon dioxide granules I or silicon dioxide granules II or both) may contain further components, for example in the form of molecules, ions or elements. The silicon dioxide granules preferably contain less than 5 ppm, for example less than 3 ppm, particularly preferably less than 1 ppm of atoms other than Si, O, H, C, Cl, preferably in an amount of at least 1 ppb, based on the total weight of the silicon dioxide granules. The further components may in particular be selected from the group consisting of carbon, fluoride, iodide, bromide, phosphorus or a mixture of at least two thereof.
[0361] The silicon dioxide granules preferably contain less than 10 ppm, for example less than 8 ppm or less than 5 ppm, particularly preferably less than 4 ppm, of carbon, in each case based on the total weight of silicon dioxide. The silicon dioxide granules often contain an amount of carbon of at least 1 ppb.
[0362] The silicon dioxide granules preferably contain less than 100 ppm, for example less than 80 ppm, particularly preferably less than 70 ppm, of other components, in each case based on the total weight of the silicon dioxide granules, but in most cases at least 1 ppb of other components.
[0363] Pretreatment step before melting The silicon dioxide granules formed in step v.) may be subjected to one or more pretreatment steps before being heated to obtain a glass melt in step vi.) The pretreatment steps may, for example, be thermal or mechanical treatment steps.
[0364] a.) Precompression The silicon dioxide granules can be, for example, compressed before heating in the course of step vi.) The term "compression" is understood to mean reducing the BET surface area and pore volume.
[0365] The silicon dioxide granules are preferably thermally treated by heating them or mechanically treated by applying pressure to them, for example by rolling or pressing them. The silicon dioxide granules are preferably compressed by heating them. Particularly preferably, the silicon dioxide granules are compressed by heating them by a preheating section connected to a melting furnace.
[0366] The silicon dioxide is preferably compressed by heating at a temperature in the range of 800 to 1400°C, for example at a temperature in the range of 850 to 1300°C, particularly preferably at a temperature in the range of 900 to 1200°C.
[0367] In a further embodiment, the BET surface area of the silicon dioxide granules before step vi.) is 5 m 2 / g, preferably less than 7m 2 / g or less than 10m 2 / g, particularly preferably less than 15m 2 / g. It is also preferred that the BET surface area of the silicon dioxide granules before step vi.) is not reduced compared to the silicon dioxide granules provided in step i.).
[0368] In a further embodiment, the BET surface area of the silicon dioxide granules is 20 m 2 / g, e.g. 15m 2 / g or less than 10m 2 / g or more than 5 to 20m 2 / g or less than 7~15m 2 / g, particularly preferably 9 to 12 m 2 The BET surface area of the silicon dioxide granules before step vi.) is preferably reduced to within 40 m 2 / g compared to the silicon dioxide granules formed in step v.). 2 / g, e.g. 1-20m 2 / g or 2 to 10m 2 / g, particularly preferably 3 to 8m 2 / g, and the BET surface area after compression is 5m 2 / g.
[0369] The compressed silicon dioxide granules preferably have at least one, for example at least two or at least three or at least four, particularly preferably at least five, of the following properties: A.5+~35m 2 / g, e.g., 10-30m 2 / g, particularly preferably 15 to 25m 2 BET surface area in the range of / g; B. Particle size D in the range of 100 to 300 μm, particularly preferably in the range of 120 to 200 μm 10 ; C. Particle size D in the range of 150 to 550 μm, particularly preferably in the range of 200 to 350 μm 50 ; D. Particle size D in the range of 300 to 650 μm, particularly preferably in the range of 400 to 500 μm 90 ; E. 0.7 to 1.6 g / cm or 0.8 to 1.2 g / cm 3, particularly preferably 1.0 to 1.4 g / cm 3 Bulk density in the range of; F.1.0~1.4g / cm 3 , particularly preferably 1.15 to 1.35 g / cm 3 Tap density in the range of; G. A carbon content of less than 5 ppm, for example less than 4.5 ppm, particularly preferably less than 4 ppm; H. a chlorine content of less than 500 ppm, particularly preferably 1 ppb to 200 ppm; Here, ppm and ppb are in each case based on the total weight of the compressed silicon dioxide granules.
[0370] The compressed silicon dioxide granules preferably have a combination of properties A. / F. / G. or A. / F. / H. or A. / G. / H., particularly preferably a combination of properties A. / F. / G. / H.
[0371] The compressed silicon dioxide granules preferably have a combination of properties A. / F. / G. and a BET surface area of 10 to 30 m 2 / g range, tap density is in the range of 1.15-1.35 g / ml, and carbon content is less than 4 ppm.
[0372] The compressed silicon dioxide granules preferably have a combination of properties A. / F. / H. and a BET surface area of 10 to 30 m 2 / g, tap density is in the range of 1.15 to 1.35 g / ml, and chlorine content is in the range of 1 ppb to 200 ppm.
[0373] The compressed silicon dioxide granules preferably have a combination of properties A. / G. / H. and a BET surface area of 10 to 30 m 2 / g, the carbon content is less than 4 ppm, and the chlorine content is in the range of 1 ppb to 200 ppm.
[0374] The compressed silicon dioxide granules preferably have a combination of properties A. / F. / G. / H. and a BET surface area of 10 to 30 m 2 / g range, tap density is in the range of 1.15 to 1.35 g / ml, carbon content is less than 4 ppm, and carbon content is in the range of 1 ppb to 200 ppm.
[0375] b.) Addition of silicon compounds Silicon components other than silicon dioxide can be added in at least one step of the process for producing the quartz glass body. Hereinafter, the addition of silicon components other than silicon dioxide is also referred to as Si doping.
[0376] The silicon component other than silicon dioxide can in principle be added in any desired form, for example as a solid, liquid, gas, solution or dispersion. The silicon component other than silicon dioxide is preferably added as a powder. The powder or silicon dioxide component other than silicon dioxide preferably has an average particle size of up to 10 mm, for example up to 1000 μm, up to 400 μm, or in the range of 1 to 400 μm, for example 2 to 200 μm or 3 to 100 μm, particularly preferably 1 to 50 μm or 2 to 20 μm. The particle size data is based on the state of the silicon component other than silicon dioxide at room temperature. In a preferred alternative embodiment, the silicon component other than silicon dioxide can be added as a liquid or gas.
[0377] Silicon components other than silicon dioxide are preferably added in an amount in the range of 1 to 100,000 ppm, for example in the range of 10 to 10,000 ppm or in the range of 30 to 1000 ppm, or in the range of 50 to 500 ppm, particularly preferably in the range of 80 to 200 ppm, and further particularly preferably in the range of 200 to 300 ppm, where ppm is in each case based on the total weight of silicon dioxide.
[0378] The silicon components other than silicon dioxide preferably have a purity of at least 99.5% by weight, for example at least 99.8% by weight, or at least 99.9% by weight, or at least 99.99% by weight, particularly preferably at least 99.999% by weight, in each case based on the total weight of the silicon components.
[0379] Silicon components other than silicon dioxide preferably have a carbon content of 10 ppm or less, for example 50 ppm or less, particularly preferably 1 ppm or less, in each case based on the total weight of the silicon components.
[0380] The silicon component other than silicon dioxide is preferably selected from silicon, silicon-hydrogen compounds, silicon-oxygen compounds, or silicon-hydrogen-oxygen compounds. The silicon component other than silicon dioxide is preferably selected from silicon, silicon-hydrogen compounds, silicon-oxygen compounds, or silicon-hydrogen-oxygen compounds. The silicon component other than silicon dioxide is preferably elemental silicon.
[0381] The silicon component other than silicon dioxide preferably contains contaminants selected from the group comprising Al, Ca, Co, Cr, Cu, Fe, Ge, Hf, K, Li, Mg, Mn, Mo, Na, Nb, Ni, Ti, V, W, Zn, Zr in an amount of 250 ppm or less, for example 150 ppm or less, particularly preferably 100 ppm or less, in each case based on the total weight of the silicon component. This applies particularly preferably when the selected silicon component is silicon.
[0382] In principle, Si doping can be carried out at any step of the process. The silicon components other than silicon dioxide may already be added in process step i.) or ii.). In another embodiment, the silicon components other than silicon dioxide are added during processing of the silicon dioxide powder into silicon dioxide granules (step v.). For example, the silicon components other than silicon dioxide can be added to the silicon dioxide before, during or after granulation. Furthermore, in step vi.), the silicon components can be injected into the glass melt. However, adding them during one or more of process steps i.), ii.) and v.) is preferred over adding them in step vi.). In particular, they are added in step v.).
[0383] Preferably, the silicon dioxide powder containing the slurry can be used to add silicon components other than silicon dioxide, so that Si can be injected therein.For this purpose, for example, the silicon components other than silicon dioxide are mixed with the silicon dioxide particle powder and then slurried in a liquid, or the silicon dioxide powder is injected and slurried in a slurry or solution of silicon components other than silicon dioxide.
[0384] Preferably, silicon can be injected by adding silicon components other than silicon dioxide during granulation.In principle, silicon components other than silicon dioxide can be added at any desired time during granulation.In the case of spray granulation, silicon components other than silicon dioxide can be injected into the spray tower together with the slurry through a nozzle.In the case of rotary granulation, silicon components other than silicon dioxide can be injected in solid form or as a slurry, for example, after injecting the slurry into the stirred vessel.
[0385] More preferably, the silicon can be doped by adding silicon components other than silicon dioxide after granulation. The silicon dioxide granules can be doped by adding silicon components other than silicon dioxide while the silicon dioxide granules are further processed, preferably while the silicon dioxide is thermally or mechanically treated or when it is precompressed.
[0386] More preferably, silicon components other than silicon dioxide can be added during one or more of the above sections, in particular during and after thermal or mechanical treatment of the silicon dioxide granules or during and after precompression of the silicon dioxide granules.
[0387] The silicon component other than silicon dioxide can in principle be silicon or any silicon compound with reducing effect known to those skilled in the art.The silicon component other than silicon dioxide is preferably silicon, silicon-hydrogen compounds such as silanes, silicon-oxygen compounds such as silicon monoxide, or silicon-hydrogen-oxygen compounds such as disiloxanes.Examples of preferred silanes are monosilane, disilane, trisilane, tetrasilane, pentasilane, hexasilane, heptasilane, higher homologs and isomers of the above-listed ones, and cyclic silanes such as cyclopentasilane.Silicon is particularly preferred.
[0388] In a further embodiment, silicon components other than silicon dioxide can be added to the melting furnace together with the silicon dioxide granules. Silicon as a silicon component other than silicon dioxide can be preferably injected into the melting furnace together with the silicon dioxide granules. The silicon is preferably added as a powder, in particular with the particle size already mentioned for adding silicon components other than silicon.
[0389] Silicon components other than silicon dioxide are preferably added to the silicon dioxide granules before injection into the melting furnace. They can in principle be added at any time after the granules are formed, for example in the preheater section, before or during precompression of the silicon dioxide granules.
[0390] Silicon dioxide granules obtained by adding silicon components other than silicon dioxide are called "Si-doped granules". The Si-doped granules preferably have at least one of the following properties, for example at least two or at least three or at least four, particularly preferably at least five: [1] More than 5~40m 2 / g, e.g., 10-30m 2 / g, particularly preferably 15 to 25m 2 BET surface area in the range of / g; [2] Particle size D in the range of 100 to 300 μm, particularly preferably in the range of 120 to 200 μm 10 ; [3] Particle size D in the range of 150 to 550 μm, particularly preferably in the range of 200 to 350 μm 50 ; [4] Particle size D in the range of 300 to 650 μm, particularly preferably in the range of 400 to 500 μm 90 ; [5] 0.8~1.6g / cm 3 , particularly preferably 1.0 to 1.4 g / cm 3 Bulk density in the range of; [6] 1.0-1.4g / cm 3 , particularly preferably 1.15 to 1.35 g / cm 3 Tap density in the range of; [7] A carbon content of less than 5 ppm, for example less than 4.5 ppm, particularly preferably less than 4 ppm; [8] A chlorine content of less than 500 ppm, particularly preferably 1 ppb to 200 ppm; [9] An aluminum content of less than 200 ppb, particularly preferably 1 ppb to 100 ppb;
[10] A metal content of metals other than aluminum of less than 1000 ppb, for example in the range of 1 to 400 ppb, particularly preferably in the range of 1 to 200 ppb;
[11] Residual moisture of less than 3% by weight, for example 0.001% to 2% by weight, particularly preferably in the range of 0.01 to 1% by weight; Here, the weight percent, ppm and ppb are in each case based on the total weight of the Si-injected granulate.
[0391] Step vi.) In step vi.), a glass melt is formed from the silicon dioxide granules. This usually involves heating the silicon dioxide granules until a glass melt is obtained. Heating the silicon dioxide granules to a glass melt can in principle be carried out by any means known to those skilled in the art for this purpose.
[0392] V-Drawing for the Preparation of Glass Melts For example, the formation of a glass melt from the silicon dioxide granules by heating may be carried out by a continuous process in which the silicon dioxide granules are preferably continuously fed into the oven, or the glass melt is continuously removed from the oven, or both. The silicon dioxide granules are also preferably continuously fed into the oven, and the gas melt is continuously removed from the oven.
[0393] A suitable furnace is one that has, as a rule, at least one inlet and at least one outlet. Inlet is taken to mean an opening through which silicon dioxide and, if present, other substances can be fed into the furnace. Outlet is taken to mean an opening through which at least a portion of the silicon dioxide can be taken from the furnace. The furnace may, for example, be oriented vertically or horizontally. The furnace is preferably oriented vertically. At least one inlet is preferably above at least one outlet. In relation to the fixtures and features of the furnace, in particular the inlets and outlets, "above" means that a fixture or feature that is placed "above" another fixture has a position higher than 0 in absolute height (NN). "Vertical" is taken to mean that the direct connection between the inlet and outlet of the furnace is no more than 30° from the direction of gravity.
[0394] According to one embodiment, the furnace comprises a hanging sheet metal crucible, into which the silicon dioxide granules are fed and heated to obtain a glass melt. A sheet metal crucible is understood to mean a crucible comprising at least one rolled metal sheet. The sheet metal crucible preferably has two or more rolled metal sheets connected by suitable connections, such as rivets. A hanging sheet metal crucible is understood to mean such a sheet metal crucible arranged in a hanging manner in the furnace.
[0395] The hanging metal sheet crucible can in principle be made from any and all materials known to the skilled person that are suitable for melting silicon dioxide. Preferably, the metal sheet comprises a sintered material, for example a so-called sintered metal. "Sintered metal" is understood to mean a metal or alloy obtained by sintering a metal powder. The sintered metal can be converted into a metal sheet, for example by rolling. The sintered metal sheet crucible preferably comprises two or more or a number of metal sheets. These metal sheets can be made from rolled sintered metal.
[0396] The metal sheet in the metal sheet crucible preferably comprises at least one element selected from the group consisting of refractory metals, which is taken to mean the metals of subgroup 4 (Ti, Zr, Hf), subgroup 5 (V, Nb, Ta) and subgroup 6 (Cr, Mo, W).
[0397] The metal sheet in the metal sheet crucible preferably comprises a sintered metal selected from the group consisting of molybdenum, tungsten or a combination thereof. The metal sheet in the metal sheet crucible also preferably comprises at least one further refractory metal, particularly preferably rhenium, osmium, iridium, ruthenium or a combination of two or more thereof.
[0398] The metal sheet in the metal sheet crucible preferably comprises an alloy of molybdenum and a refractory metal or an alloy of tungsten and a refractory metal. Particularly preferred alloy metals are rhenium, osmium, iridium, ruthenium, or a combination of two or more thereof. According to a further example, the metal sheet in the metal sheet crucible is an alloy of molybdenum and tungsten, rhenium, osmium, iridium, ruthenium, or a combination of two or more thereof. For example, the metal sheet in the metal sheet crucible is an alloy of tungsten and molybdenum, rhenium, osmium, iridium, ruthenium, or a combination of two or more thereof.
[0399] The metal sheets in the above-mentioned sheet metal crucibles may preferably be coated with a refractory metal. According to one example, the metal sheets in the sheet metal crucibles are coated with rhenium, osmium, iridium, ruthenium, molybdenum and tungsten or a combination of two or more thereof.
[0400] The metal sheet and the coating preferably have different compositions. For example, a molybdenum metal sheet is coated with rhenium, osmium, iridium, ruthenium, tungsten, or any combination of two or more thereof. According to another example, a tungsten metal sheet is coated with one or more layers of rhenium, osmium, iridium, ruthenium, molybdenum, or any combination of two or more thereof. According to a further example, the metal sheet in the metal sheet crucible can include molybdenum alloyed with rhenium or tungsten alloyed with rhenium, and the inside of the crucible can be coated with one or more layers including rhenium, osmium, iridium, ruthenium, or any combination of two or more thereof.
[0401] The metal sheet in the hanging metal sheet crucible preferably has a density of 95% or more of theoretical density, for example, a density of 95% to 98% or 96% to 98%. More preferred are higher theoretical densities, especially in the range of 98% to 99.95%. The theoretical density of the active material is equal to the density of a non-porous 100% dense material. A density of the metal sheet in the metal sheet material of more than 95% can be obtained, for example, by sintering a sintered metal and then compressing the sintered material. Particularly preferably, the metal sheet crucible can be obtained by sintering a sintered metal to obtain a metal sheet and processing the metal sheet to make a crucible.
[0402] The metal sheet crucible preferably has at least a cover, a wall and a base sheet. The hanging metal sheet crucible preferably has at least one, for example at least two or at least three or at least four, particularly preferably at least five or all, of the following properties: (a) at least one layer, for example one or more or at least two or at least three or at least five, particularly preferably three or four, metal sheet layers; (b) at least one metal sheet, for example at least 3 or at least 4 or at least 6 or at least 8 or at least 12 or at least 15 or at least 16 or at least 20 metal sheets, particularly preferably 12 or 16 metal sheets; (c) at least one combination of two metal sheet parts, for example at least 2, or at least 5, or at least 10, or at least 18, or at least 24, or at least 36, or at least 48, or at least 60, or at least 72, or at least 48, or at least 96, or at least 120, or at least 160, particularly preferably 36 or 48, combinations of two identical or multiple different metal sheet parts of a hanging metal sheet crucible; (d) The metal sheet parts of the hanging sheet metal crucible are, for example, riveted in at least one combination, for example by deep drawing, for example by combining a deep drawing with a fixed metal sheet, or by air drawing, bolting or welding, for example by electron beam welding and sintering the welds, and are particularly preferably riveted. (e) the metal sheet in the hanging metal sheet crucible can be obtained by modification combined with an increase in physical density, preferably by modification of a sintered metal or sintered alloy, more preferably by modification of a rolled product; (f) a water-cooled suspension of copper, aluminum, steel, nickel or a refractory metal, such as a crucible material, preferably copper or steel; (g) a nozzle, preferably permanently connected to the crucible; (h) a mandrel, e.g., a mandrel connected to a nozzle by a step, or a mandrel attached to a cover by a handle bar, or a mandrel connected below a crucible by a handle bar; (i) at least one gas inlet, for example in the form of a filler pipe or as a separate inlet; (j) at least one gas outlet, for example as a separate outlet on the cover or in the wall of the crucible; (k) a cooling jacket, preferably a water-cooled jacket; (l) It is insulated from the outside, preferably with zirconium oxide.
[0403] The hanging sheet metal crucible can in principle be heated by any means with which the skilled person is familiar and which seems suitable for the present description. The hanging sheet metal crucible can be heated by an electric heating element (resistive) or by induction. In resistive heating, the solid surface of the sheet metal crucible is heated from the outside and transfers energy from there to its inside. In inductive heating, the energy is directly coupled by flashing to the side wall of the melting furnace and transferred from there to the inside of the furnace. In resistive heating, the energy is coupled by radiation, the solid surface is heated from the outside and transfers energy from there to its inside. The melting crucible is preferably heated by induction.
[0404] According to a further embodiment of the invention, no energy is input into the melt crucible, in particular for melting the melt, by heating the melt crucible and / or the melt therein by means of a flame, for example a burner flame in or directed towards the melt crucible. According to a further embodiment, no burner is provided for melting the melt.
[0405] The hanging metal sheet crucible can be moved in the furnace via a hanging device. Preferably, the crucible can be moved at least partially in and out of the furnace. If different heat zones are present in the furnace, their temperature profile is transferred to the crucible in the furnace, and thus changing the position of the crucible in the furnace can create multiple heat zones, variable heat zones or multiple variable heat zones in the crucible.
[0406] The metal sheet crucible has a nozzle. The nozzle is formed from a nozzle material. The nozzle material preferably comprises a precompressed material and has a density of, for example, more than 95%, for example 98-100%, particularly preferably 99-99.999%, in each case based on the theoretical density of the nozzle material. The nozzle material preferably comprises a refractory metal, for example molybdenum, tungsten or a combination thereof with further refractory metals. Molybdenum is particularly preferred as nozzle material. Nozzles comprising molybdenum can preferably have a density of 100% of the theoretical density.
[0407] The base sheet contained in the sheet metal crucible is preferably thicker than the side of the sheet metal crucible. The base sheet is preferably of the same material as the side of the sheet metal crucible. The base sheet of the sheet metal crucible is preferably not a rolled metal sheet. The base sheet is, for example, 1.1 to 5000 times thick, or 2 to 1000 times thick, or 4 to 500 times thick, based on the wall of the sheet metal crucible in each case.
[0408] According to another embodiment, the furnace includes a hanging or stationary filter crucible in which the silicon dioxide granules are introduced and heated to obtain a glass melt.
[0409] Sintered crucible is understood to mean a crucible made of sintered material, including sintered metal, having a density of not more than 96% of the theoretical density of the metal. Sintered metal is understood to mean a metal or alloy obtained by sintering metal powder. The sintered material and sintered metal in the sintered crucible are not rolled.
[0410] The sintering material of the sintering crucible preferably has a density of 85% or more of the theoretical density of the sintering material, for example 85% to 95% or 90% to 94%, particularly preferably 91% to 93%.
[0411] The sintering material can in principle include anything known to the person skilled in the art and suitable for melting silicon dioxide. The sintering metal is preferably made of at least one element selected from the group consisting of refractory metals, graphite or graphite foil stamped materials.
[0412] The sintered material preferably comprises a first sintered metal selected from the group consisting of molybdenum, tungsten or a combination thereof. More preferably, the sintered material also comprises at least one further refractory metal other than the first sintered metal, particularly preferably a refractory metal selected from the group consisting of molybdenum, tungsten, rhenium, osmium, iridium, ruthenium or a combination of two or more thereof.
[0413] The sintered material preferably comprises an alloy of molybdenum and a refractory metal or an alloy of tungsten and a refractory metal. Particularly preferred alloy metals are rhenium, osmium, iridium, ruthenium or a combination of two or more thereof. According to a further example, the sintered material comprises an alloy of molybdenum and tungsten, rhenium, osmium, iridium, ruthenium or a combination of two or more thereof. For example, the sintered material comprises an alloy of tungsten and molybdenum, rhenium, osmium, iridium, ruthenium or a combination of two or more thereof.
[0414] According to a further embodiment, the sintered material described above can include a coating comprising a refractory metal, in particular rhenium, osmium, iridium, ruthenium, or a combination of two or more thereof. According to one example, the coating comprises rhenium, osmium, iridium, ruthenium, molybdenum, and tungsten, or a combination of two or more thereof.
[0415] The sintered material and its coating are preferably configured differently. For example, a sintered material containing molybdenum is coated with one or more layers of rhenium, osmium, iridium, ruthenium, tungsten or any combination of two or more thereof. According to another example, a sintered material containing tungsten is coated with one or more layers of rhenium, osmium, iridium, ruthenium, molybdenum or any combination of two or more thereof. According to a further example, the sintered material can include molybdenum alloyed with rhenium or tungsten alloyed with rhenium, and the inside of the crucible can be coated with one or more layers including rhenium, osmium, iridium, ruthenium or any combination of two or more thereof.
[0416] Preferably, the sintered crucible is produced by sintering the sintering material in one form. The sintered crucible can be produced in one form as a whole. It is also possible to produce individual parts of the sintered crucible in a mold and then process them into the sintered crucible. The crucible is preferably produced from two or more parts, for example from a base sheet and one or more side parts. The sides are preferably produced in one piece based on the circumference of the crucible. The sintered crucible can be produced with several sides, preferably arranged one above the other. The sides of the sintered crucible are preferably sealed by bolting or by a tongue-and-groove connection. Bolting is preferably carried out by producing sides with threads on the edges. In a tongue-and-groove connection, each of the two sides to be connected has a groove on the edge into which a tongue as a connecting third part is inserted, whereby a flush connection is formed perpendicular to the crucible wall level. Particularly preferably, the sintering furnace is produced with more than one side, for example with two or more sides, particularly preferably with one or more sides. Particularly preferably, the parts of the hanging sintering crucible are bolted. Particularly preferably, the parts of the stationary sintering crucible are connected by means of a tongue and groove connection.
[0417] The base sheet can in principle be connected to the crucible wall by any means known to the skilled person suitable for this purpose. According to one embodiment, the base sheet is provided with an external thread and is connected to the crucible wall by bolting the base sheet to the crucible wall. According to a further embodiment, the base sheet is connected to the crucible wall by bolts. According to a further embodiment, the base sheet is suspended in the sintering crucible, for example by placing the base sheet on an inner flange on the crucible wall. According to a further embodiment, at least a part of the crucible wall and the thickened base sheet are sintered together. Particularly preferably, the base sheet and the crucible wall of the hanging sintering crucible are bolted. Particularly preferably, the base sheet and the crucible wall of the stationary sintering crucible are connected by a tongue and groove connection.
[0418] The base sheet contained in the sintering crucible is preferably thicker than the side walls, for example 1.1 to 20 times thicker, or 1.2 to 10 times thicker, or 1.5 to 7 times thicker, particularly preferably 2 to 5 times thicker. Preferably, the side walls over the circumference and height of the sintering crucible have a constant wall thickness.
[0419] The sintering furnace has a nozzle. The nozzle is formed from a nozzle material. The nozzle material preferably comprises a pre-compressed material and has a density of, for example, more than 95%, for example 98-100%, particularly preferably 99-99.999%, in each case based on the theoretical density of the nozzle material. The nozzle material preferably comprises a refractory metal, for example molybdenum, tungsten or a combination thereof with a refractory metal. Molybdenum is particularly preferred as the nozzle material. Nozzles comprising molybdenum can preferably have a density of 100% of the theoretical density.
[0420] The suspended sintering crucible can in principle be heated by any means with which the skilled person is familiar and which seems suitable for the purpose. The stationary sintering crucible can be heated, for example, by induction or resistance heating. In induction heating, energy is input directly to the side wall of the sintering crucible via a coil and is transferred from there to the inside of the crucible. In resistance heating, energy is input via radiation, a solid surface is heated from the outside and energy is transferred from there to its inside. The sintering furnace is preferably heated by induction.
[0421] According to a further embodiment of the invention, energy is not input into the melting crucible, in particular by heating the melting crucible or the melt it contains, for example by a flame within the melting crucible or a burner flame directed towards the melting crucible, in order to melt the melt.
[0422] Preferably, the sintering crucible has one or more heating zones, for example one or two or three or more heating zones, preferably one or two or three heating zones, in particular one heating zone. The sintering crucible heating zones can be at the same or different temperatures. For example, all heating zones can be at one temperature, all heating zones can be at different temperatures, or two or more heating zones can be at one temperature and one or more heating zones can be at another temperature independently of each other. Preferably, all heating zones are at different temperatures, for example the heating zone temperature increases in the direction in which the silicon dioxide granules are conveyed.
[0423] A suspended sintering crucible is understood to mean a sintering crucible of the above-mentioned type arranged suspended in a furnace.
[0424] The hanging sintering crucible preferably has at least one, for example two, or at least three, or at least four, particularly preferably all, of the following properties: {a} A suspension, preferably a height-adjustable suspension; {b} at least two sealed rings as sides, preferably at least two rings bolted together as sides; {c} A nozzle, preferably a nozzle permanently connected to the crucible; {d} A mandrel, for example a mandrel attached to the nozzle by a step, or a mandrel attached to the cover by a handle, or a mandrel connected below the crucible by a handle; {e} at least one gas inlet, for example in the form of a filler pipe, or at least one gas inlet, for example in the form of a filler pipe or as a separate inlet, particularly preferably in the form of a filler pipe; {f} At least one gas outlet, for example on the cover or in the wall of the crucible; {g} Cooling jacket, particularly preferably a water-cooled jacket; {h} An insulation layer on the outside of the crucible, e.g. the outside of the cooling jacket, preferably an insulation layer of zirconium oxide.
[0425] Preferred suspensions are suspensions that are fixed when producing a hanging sintering crucible, for example suspensions of the sintering material that are provided as an integral part of the crucible. Further preferred suspensions are suspensions fixed to the sintering crucible from a material other than the sintering material, for example aluminum, steel, iron, nickel or copper, preferably copper, particularly preferably cooled, for example water-cooled, copper suspensions fixed to the sintering crucible.
[0426] The hanging sintering crucible can be moved in the furnace by a hanging device. The crucible can preferably be moved at least partially in and out of the furnace. If different thermal zones are present in the furnace, their temperature profile is transferred to the crucible in the furnace, and thus changing the position of the crucible in the furnace can create multiple thermal zones, changing thermal zones, or multiple changing thermal zones in the crucible.
[0427] A stationary sintering crucible is understood to mean a sintering crucible of the abovementioned type which is placed upright in a furnace.
[0428] The stationary sintered crucible preferably has at least one, for example at least two or at least three or at least four, particularly preferably all, of the following properties: / a / an area formed as a fixing surface, preferably an area formed as a fixing surface at the bottom of the crucible, more preferably an area formed as a fixing surface at the base sheet of the crucible, particularly preferably an area formed as a fixing surface at the outer edge of the bottom of the crucible; / b / at least two sealed rings as sides, preferably at least two rings sealed by tongue and groove connections as sides; / c / nozzle, preferably a nozzle permanently connected to the furnace, particularly preferably in the area of the base of the crucible that is not formed as a fixed surface; / d / Mandrel, for example a mandrel attached to the nozzle by a step, or a mandrel attached to the cover by a step, or a mandrel connected under the crucible by a handle; / e / At least one gas inlet, for example in the form of a filler pipe or as a separate inlet; / f / at least one gas outlet, for example as a separate outlet on the cover or in the wall of the furnace; / g / Cover.
[0429] The stationary sintering crucible preferably has a separation of the gas chamber in the furnace and in the area below the furnace. The area below the furnace is taken to mean the area below the nozzle where the entrained glass melt is found. Preferably, the gas chamber is separated by the area where the crucible is placed. The gas in the gas chamber of the furnace between the inner wall of the furnace and the outer wall of the crucible cannot escape to the area below the furnace. The removed glass melt does not come into contact with the gas from the gas chamber of the furnace. The glass melt removed from the furnace with the stationary sintering crucible and the quartz glass body made therefrom preferably have a higher surface purity than the glass melt removed from the furnace with the hanging sintering crucible and the quartz glass body made therefrom.
[0430] In all preferred embodiments of the crucible, the crucible is connected to the inlet and outlet of the furnace so that the silicon dioxide granules can enter the crucible through the crucible inlet and the furnace inlet and can be removed through the crucible outlet and the furnace outlet.
[0431] Adjacent to the at least one inlet, the crucible has at least one opening, preferably a plurality of openings, through which gas can be supplied and discharged. The crucible preferably has at least two openings, at least one of which can be used as a gas inlet and at least one of which can be used as a gas outlet. By using at least one opening as a gas inlet and at least one opening as a gas outlet, a gas flow is preferably generated within the crucible.
[0432] The silicon dioxide granules are fed into the crucible through the crucible inlet and then heated in the crucible. The heating can be carried out in the presence of a gas or a mixture of two or more gases. When heated, the water bound in the silicon dioxide granules can be transferred to the gas phase to form further gas. The gas or the mixture of two or more gases is in the gas chamber of the crucible. Below the gas chamber of the crucible is understood to mean the inner area of the crucible that is not occupied by the solid or liquid phase. Suitable gases are, for example, hydrogen, inert gases and two or more thereof. "Inert gas" is understood to mean a gas that does not react with the substance provided in the crucible at a temperature of up to 2400 ° C. Preferred inert gases are nitrogen, helium, neon, argon, krypton and xenon, particularly preferably argon and helium. The heating is preferably carried out in a reducing atmosphere. This can be preferably provided by hydrogen or a combination of hydrogen with an inert gas, for example a combination of hydrogen with helium, or a combination of hydrogen with nitrogen, or a combination of hydrogen with argon, particularly preferably a combination of hydrogen with helium.
[0433] Preferably, at least partial gas exchange of air, oxygen and water is carried out in the silicon dioxide granules with hydrogen, at least one inert gas, or with a combination of hydrogen and at least one inert gas. At least partial gas exchange is carried out in the silicon dioxide granules when injecting the silicon dioxide granules, or before heating, or during heating, or during at least two of the above activities. The silicon dioxide granules are preferably heated until melted in a gas flow of hydrogen and at least one inert gas, such as argon or helium.
[0434] Preferably, all embodiments of the furnace have a melting crucible and at least one gas inlet through which the gas that is fed through the furnace and formed when the furnace is operated is taken out. The furnace may also have at least one dedicated gas inlet. Alternatively or additionally, the gas may be injected through a solid feed, also known as a solid inlet, for example together with the silicon dioxide granules, or before, after or through a combination of two or more of the aforementioned options.
[0435] The oven and gas flow are preferably characterized by the properties described in connection with the first problem. The gas flow is preferably generated by injecting gas into the oven through an inlet and removing gas from the oven through an outlet. The term "gas exchange rate" is understood to mean the volume of gas passing from the oven to the outlet per unit time. The gas exchange rate is also called gas flow throughput or volumetric throughput.
[0436] The gas flow gas exchange rate is preferably in the range of 200 to 3000 l / h, for example 200 to 2000 l / h, particularly preferably 200 to 1000 l / h.
[0437] The furnace temperature for melting the silicon dioxide granules is preferably in the range of 1700 to 2500 ° C, for example in the range of 1900 to 2400 ° C, particularly preferably in the range of 2100 to 2300 ° C.
[0438] The residence time in the furnace is preferably in the range of 1 hour to 50 hours, for example 1 to 30 hours, particularly preferably 5 to 20 hours. In the present context, "residence time" means the time required during the process to remove the charge from the melting furnace in which the glass melt is formed. The charge is the total mass of silicon dioxide present in the melting furnace. Here, the silicon dioxide may be present both as a solid and as a glass melt.
[0439] The furnace temperature is preferably increased over the length in the direction in which the material is conveyed. The furnace temperature is preferably increased by at least 100° C., for example at least 300° C., or at least 500° C., or at least 700° C., particularly preferably at least 1000° C., over the length in which the material is conveyed. The maximum temperature in the furnace is preferably 1700-2500° C., for example 1900-2400° C., particularly preferably 2100-2300° C. The furnace temperature can be increased uniformly or according to a temperature profile.
[0440] The furnace temperature is preferably reduced before the glass melt is removed from the furnace. The furnace temperature is preferably reduced by 50 to 500°C, for example 100°C or 400°C, particularly preferably 150 to 300°C, before the glass melt is removed from the furnace. The temperature of the glass melt at the time of removal is preferably 1750 to 2100°C, for example 1850 to 2050°C, particularly preferably 1900 to 2000°C.
[0441] The furnace temperature is preferably reduced over the length in the direction of conveying the material before the glass melt is removed from the furnace. The furnace temperature is preferably reduced by at least 100° C., for example by at least 300° C., or at least 500° C., or at least 700° C., particularly preferably by at least 1000° C., over the length in which the material is conveyed. The maximum temperature in the furnace is 1700-2500° C., for example by 1900-2400° C., particularly preferably by 2100-2300° C. The furnace temperature is preferably reduced by 50-500° C., for example by 100° C. or 400° C., particularly preferably by 150-300° C., before the glass melt is removed from the furnace.
[0442] Preheat Section The furnace preferably has at least a first chamber and a further chamber connected to each other by a throughput, the first chamber and the further chamber being at different temperatures, the temperature of the first chamber being lower than that of the further chamber. In the further chamber, a glass melt is formed from the silicon dioxide granules. Hereinafter, this chamber is called the melting chamber. The chamber connected to the melting chamber via the material supply, but upstream of it, is also called the preheating section. This is, for example, one in which at least one outlet is directly connected to the inlet of the melting chamber. The arrangement can also be formed in an independent furnace, in which case the melting chamber is a melting furnace. However, for the sake of further explanation, the melting furnace and the melting chamber may be interpreted as synonymous, and therefore what is said about the melting furnace also applies to the melting chamber and vice versa. The term "preheating section" is the same in both cases.
[0443] The silicon dioxide granules are preferably at a temperature in the range of 20 to 1300 ° C when they enter the furnace.
[0444] According to the first embodiment, the silicon dioxide granules are not tempered before entering the melting chamber. For example, when the silicon dioxide granules enter the oven, they have a temperature in the range of 20 to 40 ° C, particularly preferably 20 to 30 ° C. If the silicon dioxide granules II are prepared according to step i.), the silicon dioxide granules II preferably have a temperature in the range of 20 to 40 ° C, particularly preferably 20 to 30 ° C, when they enter the oven.
[0445] According to another embodiment, before entering the furnace, the silicon dioxide granules are tempered to a temperature in the range of 40-1300 ° C. Tempering means setting the temperature to a selected value. Tempering can in principle be carried out by any and all means known to a person skilled in the art for tempering silicon dioxide granules. For example, tempering can be carried out in a furnace arranged separately from the melting chamber or in a furnace connected to the melting chamber.
[0446] The tempering is preferably carried out in a chamber connected to the melting chamber. That is, the furnace comprises a preheating section in which the silicon dioxide can be tempered. Preferably, the preheating section itself is a moving furnace, particularly preferably a rotary furnace. The rotary furnace is understood to mean a heating chamber that moves the silicon dioxide from the inlet of the moving furnace to the outlet of the moving furnace during operation. The outlet is preferably directly connected to the inlet of the melting furnace, so that the silicon dioxide granules can enter the melting furnace from the preheating section without further intermediate steps or operations.
[0447] The preheating section also preferably has at least one gas inlet and at least one gas outlet. Gas can enter the gas chamber of the preheating section through the gas inlet and exit through the gas outlet. It is also possible to inject gas into the preheating section through the inlet silicon dioxide granules. Similarly, the gas can be discharged through the preheating section outlet and then separated from the silicon dioxide granules. Preferably, the gas can be supplied to the preheating section through the silicon dioxide granules inlet and the gas inlet and discharged through the preheating section outlet and the preheating section gas outlet.
[0448] A gas flow is preferably generated in the preheating section using a gas inlet and a gas outlet. Suitable gases are hydrogen, an inert gas and two or more thereof. Preferred inert gases are nitrogen, helium, neon, argon, krypton and xenon, particularly preferably nitrogen and helium. The preheating section preferably has a reducing atmosphere. This can be preferably provided by hydrogen or a combination of hydrogen and an inert gas, for example a combination of hydrogen and helium or a combination of hydrogen and nitrogen, particularly preferably a combination of hydrogen and helium. The preheating section also preferably has an oxidizing atmosphere. This can preferably be provided by oxygen or a combination of oxygen and one or more other gases, air being particularly preferred. It is also possible to temper the silicon dioxide in the preheating section under reduced pressure, preferably.
[0449] When entering the oven, for example, the silicon dioxide granules have a temperature in the range of 100 to 1100 ° C, or 300 to 1000 or 600 to 900 ° C.
[0450] According to one embodiment of the first subject, the furnace comprises at least two chambers. The furnace preferably comprises a first chamber and at least one further chamber. The first chamber and the further chamber are connected to each other via a passage.
[0451] At least two chambers in the furnace can in principle be arranged as desired, preferably vertically or horizontally, particularly preferably vertically. The chambers in the furnace are preferably arranged such that when carrying out the process according to the first subject, the silicon dioxide granules pass through the first chamber and then through the further chamber to obtain a glass melt. The further chamber preferably has the characteristics of the melting furnace and the crucible arranged therein described above.
[0452] Preferably, each of the chambers has an inlet and an outlet. The furnace inlet is preferably connected to the inlet of the first chamber via a passage. The furnace outlet is preferably connected to the outlet of the further chamber via a passage. The outlet of the first chamber is preferably connected to the inlet of the further chamber via a passage.
[0453] The chamber is preferably arranged in the oven so that the silicon dioxide granules can reach the first chamber. The chamber is preferably arranged in the oven so that the silicon dioxide glass melt can be removed from the further chamber via the oven outlet. Particularly preferably, the silicon dioxide granules can reach the first chamber via the oven inlet and the silicon dioxide melt can be removed from the further chamber via the oven outlet.
[0454] Silicon dioxide can be obtained from the passage from the first chamber to the further chamber as granules or powder in the direction in which the material specified in the method is conveyed. The chambers connected via the passage include an arrangement in which a further element is arranged between the first chamber and the further chamber in the direction in which the material is conveyed. Gases, liquids and solids can in principle pass through the passage. The suspension of silicon dioxide powder, silicon dioxide powder and silicon dioxide granules can preferably pass through the transition between the first chamber and the further chamber. During the procedure according to the invention, all substances introduced into the input to the first chamber can enter the further chamber via the passage between the first chamber and the further chamber. Preferably, only silicon dioxide in the form of granules or powder enters the further chamber via the passage. Preferably, the passage between the first chamber and the further chamber is sealed by silicon dioxide so that the gas chambers of the first chamber and the further chamber are separated from each other, preferably so that the gas chambers can contain different gases or gas mixtures, different pressures or both. According to another embodiment, the passage is formed from a sluice, preferably a porous wheel sluice.
[0455] The first chamber of the furnace preferably has at least one gas inlet and at least one gas outlet. The gas inlet can in principle take any form known to the skilled person and suitable for injecting gas, for example a nozzle, a valve or a pipe. The gas outlet can in principle take any form known to the skilled person and suitable for removing gas, for example a nozzle, a valve or a pipe.
[0456] Preferably, the silicon dioxide granules are introduced into the first chamber and heated through the oven inlet, and may be heated in the presence of a gas or a combination of two or more gases. For this, the gas or a combination of two or more gases is in the first chamber. The gas chamber of the first chamber is taken to mean the area of the first chamber that is not occupied by a solid or liquid phase. Suitable gases are, for example, hydrogen, oxygen, an inert gas or two or more thereof. Preferred inert gases are nitrogen, helium, neon, argon, krypton and xenon, particularly preferred are nitrogen, helium or a combination thereof. The heating is preferably carried out in a reducing atmosphere. This can preferably be provided by hydrogen or a combination of hydrogen and helium. The silicon dioxide granules are preferably heated in the first chamber in a gas flow or a combination of two or more gases.
[0457] It is further preferred that the silicon dioxide granules are heated in the first chamber under reduced pressure, for example at a pressure of less than 500 mbar or less than 300 mbar, for example less than or equal to 200 mbar.
[0458] Preferably, the first chamber is provided with at least one device for moving the silicon dioxide granules. In principle, any device known to those skilled in the art and deemed suitable for this purpose can be selected. Preferably, stirring, shaking or rocking devices are suitable.
[0459] According to a further embodiment, the temperatures in the first chamber and in the further chamber are different. The temperature in the first chamber is preferably lower than the temperature in the further chamber. The temperature difference between the first chamber and the further chamber is preferably in the range of 600-2400°C, for example in the range of 1000-2000°C or 1200-1800°C, particularly preferably in the range of 1500-1700°C. Furthermore, the temperature in the first chamber is preferably lower than the temperature in the further chamber by 600-2400°C, for example in the range of 1000-2000°C or 1200-1800°C, particularly preferably by 1500-1700°C.
[0460] According to a further embodiment, the first chamber of the furnace is a preheating section, particularly preferably a preheating section as described above, having the above-mentioned characteristics. The preheating section is preferably connected to the first chamber via a passage. The silicon dioxide from the preheating section preferably enters the further chamber via a passage. The passage between the preheating section and the further chamber can be closed so that the gas injected into the preheating section cannot enter the further chamber through the passage. The passage between the preheating section and the further chamber is closed so that the silicon dioxide does not come into contact with water. The passage between the preheating section and the further chamber can be closed so that the gas chamber of the preheating section and the first chamber are separated from each other and the gas chamber can contain different gases or gas mixtures or both. Suitable passages are preferably the above-mentioned embodiments.
[0461] According to a further embodiment, the first chamber of the furnace is not a preheating section. For example, the first chamber is an equalization chamber. An equalization chamber is understood to mean a chamber of the furnace in which throughput fluctuations in the upstream preheating section or throughput differences between the preheating section and the further chamber are equalized. For example, as mentioned above, a rotary furnace can be provided upstream of the first chamber. This usually has a throughput that can vary up to 6% of the average throughput. In the equalization chamber, the silicon dioxide is preferably kept at the temperature at which it enters the equalization chamber.
[0462] It is also possible for the furnace to have a first chamber and one or more further chambers, for example two further chambers or three further chambers or four further chambers or five further chambers or more than five further chambers, particularly preferably two further chambers. If the furnace has two further chambers, based on the direction in which the material is transported, the first chamber is preferably a preheating section, a first of the further chambers is an equalization chamber and a second of the further chambers is a melting chamber.
[0463] According to a further embodiment, an additive is present in the first chamber, preferably selected from the group consisting of a halogen, an inert gas, a base, oxygen or a combination of two or more thereof.
[0464] Suitable additives are in principle halogens in elemental form and halogen compounds. The halogens are preferably selected from the group consisting of chlorine, fluorine, chlorine compounds and fluorine compounds. Particularly preferred are elemental chlorine and hydrogen chloride.
[0465] Suitable additives are in principle all inert gases and mixtures of two or more of them. Preferred inert gases are nitrogen, helium or combinations thereof.
[0466] In principle, bases are also suitable additives. Preferred bases as additives are organic and inorganic bases.
[0467] Oxygen is also suitable as an additive, which is preferably present in an oxygen-based atmosphere, for example in combination with an inert gas or a mixture of two or more inert gases, particularly preferably in combination with nitrogen, helium or nitrogen and helium.
[0468] The first chamber can in principle comprise any material known to those skilled in the art that is suitable for heating silicon dioxide. The first chamber preferably comprises at least one element selected from the group consisting of quartz glass, refractory metal, aluminum, and combinations of two or more thereof. The first chamber preferably comprises quartz glass or aluminum.
[0469] Preferably, if the first chamber contains a polymer or aluminum, the temperature in the first chamber does not exceed 600° C. If the first chamber contains quartz glass, the temperature in the first chamber is preferably between 100 and 1100° C. The first chamber preferably essentially contains quartz glass.
[0470] When silicon dioxide is conveyed from the first chamber to the further chamber through the passage between the first chamber and the further chamber, the silicon dioxide can in principle be in any desired state.The silicon dioxide is preferably present as a solid, for example as a particle, powder or granule.According to one embodiment of the first subject, the silicon dioxide is conveyed from the first chamber to the further chamber as a granule.
[0471] According to a further embodiment, the further chamber is a metal sheet or a crucible of sintered material containing a sintered metal, the metal sheet or the sintered metal being selected from the group consisting of molybdenum, tungsten or a combination thereof.
[0472] Dew point measurement Dew point is taken to mean the temperature at which a portion of the gas or gas mixture being tested will condense without a change in pressure. This is generally taken to mean the condensation of water. The dew point is determined according to the test method described in the Methods section.
[0473] According to the invention, the dew point of the gas is below 0° C. when it leaves the furnace through the gas outlet.
[0474] According to the present invention, the furnace, preferably the melting crucible it contains, has at least one gas outlet through which the gas that is injected into the furnace and formed when using the furnace is taken out. The furnace can also have at least one dedicated gas output. Alternatively or additionally, the gas can be injected through a solid supply, also known as a solid inlet, for example together with, before, after the silicon dioxide granules, or through a combination of two or more of the options.
[0475] According to the invention, when the gas leaves the furnace via the gas outlet, the gas taken from the furnace has a dew point below 0° C., for example below −10° C. or below −20° C. The dew point is determined according to the test method described in the methods section at a slight overpressure of 5 to 20 mbar. A suitable test device is, for example, the “Optidew” device by Michell Instruments GmbH, D-61381 Friedrichsdorf.
[0476] The dew point of the gas is preferably determined at a measuring point that is at least 10 cm away from the gas outlet of the oven. This distance is often between 10 cm and 5 m. In this distance range, described herein as "at the outlet", the distance between the measuring points at the gas outlet of the oven is not critical for the dew point measurement result. The gas is supplied from the outlet to the measuring point by liquid means, for example a hose or a pipe. The temperature of the gas at the measuring point is often between 10 and 60°C, for example between 20 and 50°C, in particular between 20 and 30°C.
[0477] Suitable gases and gas mixtures have been described above. In the course of testing, it was found that the above data apply to each of the mentioned gases and gas mixtures.
[0478] According to a further preferred embodiment, before the gas or gas mixture enters the furnace, in particular the melting crucible, it has a dew point below -50°C, for example below -60°C, or below -70°C, or below -80°C. The dew point is usually below -60°C. The following ranges for the dew point on entering the furnace are also preferred: -50 to -100°C, -60 to -100°C and -70 to -100°C.
[0479] According to a further preferred embodiment, the dew point of the gas before entering the furnace is at least 30° C. lower than when it leaves the melting furnace, for example at least 50° C. lower, or 60° C. lower, or even 80° C. lower. The above data apply when measuring the dew point when it leaves the melting furnace. This applies equally when measuring the dew point before entering the furnace. The distance from the measuring point to the gas inlet of the furnace is not critical here, since no source for adding moisture is provided and no condensate can form between the measuring point and the furnace.
[0480] According to a preferred embodiment, the furnace, in particular the melting crucible, is operated with a gas exchange rate in the range of 200-3000 l / h.
[0481] According to a preferred embodiment, the melting crucible is at least partially formed from a material comprising one or more metals selected from molybdenum, tungsten, wolfram, rhenium, iridium, osmium.
[0482] According to a preferred embodiment, the quartz glass body contains less than 1000 ppb in total of one or more metals selected from molybdenum, tungsten, rhenium, iridium, and osmium, where the total amount is based on the total weight of the quartz glass body.
[0483] According to a preferred embodiment, the dew point is determined in a test cell, which is separated from the gas leaving the gas outlet by a membrane. The membrane is preferably moisture permeable. This measure makes it possible to protect the test cell from any amount of dust and other particles in the gas stream that the gas stream carries from the melting furnace, in particular the melting crucible. This measure makes it possible to significantly extend the service life of the test probe. By service life is meant the period during operation of the furnace during which the test probe does not need to be replaced or cleaned.
[0484] According to a preferred embodiment, a dew point measuring device or dew point level hygrometer is used.
[0485] In one embodiment of the first task, the melt energy for carrying out step vi.) is transferred to the silicon dioxide granules via a solid surface. The silicon dioxide granules selected are, for example, compressed silicon dioxide granules.
[0486] "Solid surface" is understood to mean a surface other than the surface of the silicon dioxide granules, which does not melt or form at the temperature at which the silicon dioxide granules are heated to their melting point. Suitable materials for the solid surface are, for example, materials suitable as crucible materials.
[0487] The solid surface may in principle be any surface known to the person skilled in the art and suitable for these purposes. The solid surface used may be the solid surface of a crucible or a separate component that is not a furnace.
[0488] The solid surface can in principle be heated by any means known to those skilled in the art and suitable for these purposes to transfer melting energy to the silicon dioxide granules. The solid surface is preferably heated by resistance heating or induction heating. In induction heating, energy is input directly to the solid surface via a coil and then transferred to the inside of the solid surface. In resistance heating, the solid surface is heated from the outside and transfers energy from there to its inside, and a heating chamber gas with low heating capacity, for example an argon atmosphere or an argon-containing atmosphere, is advantageous. The solid surface can be heated, for example, electrically or by sintering the solid surface with an external flame. The solid surface is preferably heated to a temperature that can transfer a sufficient amount of energy to the silicon dioxide granules and / or the already partially melted silicon dioxide granules are heated to a temperature sufficient to melt the silicon dioxide granules.
[0489] According to one embodiment of the present invention, no energy is introduced into the crucible at least during step vi.) by heating the crucible or the melt it contains or both, for example by means of a flame, such as a burner flame directed in or on the crucible.
[0490] When a separate component is used as the solid surface, it can be contacted with the silicon dioxide granules by any desired means, for example, by placing the component on the silicon dioxide granules, or by inserting the component between the silicon dioxide granules, or by inserting the component between the crucible and the silicon dioxide granules, or by a combination of two or more thereof. The component can be before or during, or before and during, the transfer of melting energy.
[0491] The melting energy is preferably transferred to the silicon dioxide granules through the inside of the crucible, heating the crucible to a point where the silicon dioxide granules melt. The crucible is preferably resistively or inductively heated. Heat is transferred from the outside to the inside of the crucible. The solid surface inside the crucible transfers the melting energy to the silicon dioxide granules.
[0492] According to a further embodiment, the melting energy is not transferred to the silicon dioxide granules through the gas chamber.Furthermore, the melting energy is not transferred to the silicon dioxide granules by firing the silicon dioxide granules with a flame.An example of these excluded energy transfer paths is directing one or more burner flames from above into the melting furnace, or onto the silicon dioxide, or both.
[0493] Step vii.) The glass melt is removed from the furnace via an outlet, preferably via a nozzle. The quartz glass body is formed by removing at least a portion of the glass melt, preferably the glass melt produced in step vi.).
[0494] The removal of the part of the glass melt produced in step vi) can in principle take place continuously from the melting furnace or melting chamber or after the production of the glass melt is completed. The part of the glass melt can preferably be removed continuously. The glass melt is removed via an outlet from the furnace or an outlet of the melting chamber, preferably in each case via a nozzle.
[0495] The glass melt may be cooled before, during or after its removal to a temperature at which the glass melt can be formed. Cooling the glass melt increases its viscosity. The glass melt is preferably cooled to a point where the formed shape remains formed as formed, while at the same time the forming can be performed as quickly, reliably and with as little energy as possible. The skilled person can determine how viscous the glass melt is by varying the temperature of the glass melt in the forming tool. The glass melt when removed preferably has a temperature in the range of 1750-2100°C, for example 1850-2050°C, particularly preferably less than 1900-2000°C. After removal, the glass melt is preferably cooled to a temperature of less than 500°C, for example less than 200°C or less than 100°C or less than 50°C, particularly preferably to a temperature in the range of 20-30°C.
[0496] The formed quartz glass body may be a solid or a hollow body. A solid is taken to mean an object essentially composed of a single material, although a solid may have one or more inclusions, such as air bubbles. Such inclusions in a solid body are often found to be 65 mm or less in size. 3 The following sizes, e.g. 40mm 3 Less than or 20mm 3 Less than or 5mm 3 Less than or 2mm 3 Less than 0.5 mm, particularly preferably 3 The solid preferably contains less than 0.02% by volume, for example less than 0.01% by volume or less than 0.001% by volume of its volume as inclusions, in each case based on the total volume of the solid.
[0497] The quartz glass body has an outer shape. The term "outer shape" is understood to mean the shape of the outer edge of the cross section of the glass body. The outer shape of the quartz glass body is preferably a circular, elliptical, or polygonal cross section having three or more corners, for example 4, 5, 6, 7 or 8 corners, and the quartz glass body is particularly preferably a circular shape.
[0498] The quartz glass body preferably has a length in the range of 100 to 10,000 mm, for example, 1,000 to 4,000 mm, particularly preferably 1,200 to 3,000 mm.
[0499] The quartz glass body preferably has an outer diameter in the range of 1 to 500 mm, for example, in the range of 2 to 400 mm, and particularly preferably in the range of 5 to 300 mm.
[0500] The quartz glass body is formed by a nozzle. For this, the glass melt is fed through the nozzle. The outer shape of the quartz glass body formed through the nozzle is determined by the shape of the nozzle opening. If the nozzle opening is circular, the quartz glass body forms a cylinder when formed. If the nozzle opening has a structure, this structure is transferred to the outer shape of the quartz glass body. The quartz glass body formed using a nozzle with a structured opening shows the shape of its structure in the axial direction relative to the glass distortion.
[0501] The nozzle is incorporated into the melting furnace, preferably as part of the crucible, and most preferably as part of the outlet of the crucible.
[0502] At least a portion of the glass melt is preferably removed from the melting furnace through a nozzle. The outline of the quartz glass body is formed by removing at least a portion of the glass melt through a nozzle.
[0503] The quartz glass body is preferably cooled after it has been formed to retain its shape. Once formed, the quartz glass body is preferably cooled to a temperature at least 1000°C lower than the temperature of the glass melt at which it was formed, for example at least 1500°C or at least 1800°C, particularly preferably 1900-1950°C. The quartz glass body is preferably cooled to a temperature of less than 500°C, for example less than 200°C or less than 100°C or less than 50°C, particularly preferably to a temperature in the range of 20-30°C.
[0504] According to one embodiment, the obtained quartz glass body may be treated by at least one means selected from the group consisting of chemical, thermal or mechanical treatments.
[0505] The quartz glass body is preferably chemically post-treated. Post-treatment refers to the treatment of an already formed quartz glass body. In principle, chemically post-treating the quartz glass body is understood to mean any means known to those skilled in the art that may be suitable for changing the chemical structure or composition, or both, of the surface of the quartz glass body. The chemical post-treatment preferably comprises at least one means selected from the group consisting of treatment with a fluorine compound and ultrasonic cleaning.
[0506] The fluorine compounds may in particular be hydrogen fluoride and hydrofluoric acid, for example hydrofluoric acid. The liquid preferably has a content of fluorine compounds in the range of 35-55% by weight, preferably in the range of 35-45% by weight, where the weight percentages are in each case based on the total fluid content. The remainder of 100% by weight is usually water. The water selected is preferably fully demineralized or deionized water.
[0507] Ultrasonic cleaning is preferably carried out in a fluid bath, particularly preferably in the presence of a detergent. In the case of ultrasonic cleaning, fluorine compounds such as hydrofluoric acid or hydrogen fluoride are generally not used.
[0508] The ultrasonic cleaning of the quartz glass body is preferably carried out under at least one, for example at least two, or at least three, or at least four, or at least five, particularly preferably all, of the following conditions: -Ultrasonic cleaning is carried out in a continuous process. The ultrasonic cleaning system has at least six chambers connected to each other by pipes. The residence time of the quartz glass body in each chamber can be set. The residence time of the quartz glass body in each chamber is preferably the same. The residence time in each chamber is preferably in the range of 1 to 120 minutes, for example, less than 5 minutes, or 1 to 5 minutes, or 2 to 4 minutes, or less than 60 minutes, or 10 to 60 minutes, or 20 to 50 minutes, and particularly preferably in the range of 5 to 60 minutes. A first chamber contains a base medium, preferably containing water and a base, and an ultrasonic cleaner. A third chamber contains an acidic medium, preferably containing water and an acid, and an ultrasonic cleaner. The quartz glass body is washed with water, preferably demineralized water, in the second chamber and the fourth to sixth chambers. The fourth to sixth chambers are operated as a cascade with water, preferably demineralized water, which is preferably injected only into the sixth chamber and flows from the sixth chamber into the fifth chamber and from the fifth chamber into the fourth chamber.
[0509] The quartz glass body is preferably thermally post-treated. Post-treating the quartz glass body is understood to mean, in principle, any means known to the skilled artisan that would be suitable for changing the quartz glass body by affecting its morphology or structure, or both. The thermal post-treatment preferably comprises at least one of the following means: tempering, ramming, expanding, stretching, welding, or a combination of two or more thereof. Preferably, the thermal post-treatment is carried out without the purpose of removing material.
[0510] Tempering is preferably carried out by heating the quartz glass body in a furnace, preferably to a temperature in the range of 900 to 1300 ° C, for example in the range of 900 to 1250 ° C or 1040 to 1300 ° C, particularly preferably in the range of 1000 to 1050 ° C or 1200 to 1300 ° C. The heat treatment preferably does not exceed a temperature of 1300 ° C continuously for more than 1 hour, particularly preferably the temperature of 1300 ° C is not exceeded at any time during the entire heat treatment. Tempering can in principle be carried out under reduced pressure, normal pressure or pressure, preferably under reduced pressure, particularly preferably in vacuum.
[0511] Preferably, ramming is carried out by heating the quartz glass body, preferably to a temperature of about 2100 ° C., and then reshaping the quartz glass body during a rotational movement, preferably at a rotation speed of about 60 rpm. A quartz glass body in the form of a rod can be reshaped, for example, as a cylinder by ramming.
[0512] Preferably, the quartz glass body can be expanded by blowing gas into the quartz glass body. For example, the quartz glass body can be expanded to form a large pipe. For this, the quartz glass body is preferably heated to a temperature of about 2100 ° C, and then heated in a rotary motion, preferably at a rotation speed of about 60 rpm, and the internal space is gas flushed at a defined and controlled internal pressure, preferably up to about 100 mbar. Large pipe is understood to mean a large pipe with an outer diameter of at least 500 mm.
[0513] The quartz glass body can be preferably drawn by heating the quartz glass body to a temperature of preferably about 2100° C. and then drawing the quartz glass body to a desired outer diameter at a controlled drawing rate. Light tubes can be made from, for example, quartz glass bodies.
[0514] The quartz glass body is preferably mechanically post-treated. The post-treatment of the quartz glass body is understood to mean, in principle, any means known to those skilled in the art that would be suitable for modifying the design of the quartz glass body by abrasive means that divide the quartz glass body into two or more pieces. In particular, the mechanical post-treatment comprises at least one means selected from the group consisting of grinding, drilling, honing, sawing, water beam cutting, laser beam cutting, sandblast roughening or a combination of two or more thereof.
[0515] The quartz glass body is preferably treated with a combination of these means, for example with a combination of chemical and thermal post-treatment, or with a combination of chemical and mechanical post-treatment, or with a combination of thermal and mechanical post-treatment, particularly preferably with a combination of chemical, thermal and mechanical post-treatment. More preferably, the quartz glass body can be subjected to one or more of the above means, in each case independently of each other.
[0516] According to further embodiments, the process may include the following optional process steps: viii.) forming a hollow body having at least one opening from the quartz glass body.
[0517] The hollow body formed has an internal and external shape. "Internal shape" is understood to mean the shape of the inner edge of the hollow body when viewed in cross section. The internal and external shapes of the cross section of the hollow body may be the same or different. The cross section of the internal and external shapes of the hollow body may be circular, elliptical or polygonal with three or more corners, for example four, five, six, seven or eight corners.
[0518] The outer cross-sectional shape preferably corresponds to the inner cross-sectional shape of the hollow body. Particularly preferably, the hollow body has a circular inner cross-sectional shape and a circular outer cross-sectional shape.
[0519] In another embodiment, the internal and external shapes of the hollow body may differ from each other. The hollow body preferably has a circular external shape and a polygonal internal shape in cross section. Particularly preferably, the hollow body has a circular external shape and a hexagonal internal shape in cross section.
[0520] The length of the hollow body is preferably 100 to 10,000 mm, for example, 1,000 to 4,000 mm, particularly preferably 1,200 to 2,000 mm.
[0521] The hollow bodies preferably have a wall thickness in the range from 0.8 to 50 mm, for example in the range from 1 to 40 mm or from 2 to 30 mm or from 3 to 20 mm, particularly preferably in the range from 4 to 10 mm.
[0522] The hollow body preferably has an outer diameter in the range of 2.6 to 400 mm, for example 3.5 to 450 mm, particularly preferably 5 to 300 mm.
[0523] The hollow body preferably has an inner diameter in the range of 1 to 300 mm, for example 5 to 280 mm or 10 to 200 mm, particularly preferably in the range of 20 to 100 mm.
[0524] The hollow body comprises one or more openings. The hollow body preferably comprises one opening. The hollow body preferably comprises an even number of openings, for example 2, 4, 6, 8, 10, 12, 14, 16, 18 or 20 openings. The hollow body preferably comprises two openings. The hollow body is preferably a pipe. This form of the hollow body is particularly preferred when the light guide comprises only one core. The hollow body may comprise more than two openings. The openings are preferably in pairs opposite each other at the ends of the quartz glass body. For example, each end of the quartz glass body has two, three, four, five, six, seven or more openings, particularly preferably five, six or seven openings. Preferred forms are, for example, pipes, twin pipes, i.e. pipes with two parallel channels, multichannel rods, i.e. pipes with more than two parallel ducts.
[0525] The hollow body can in principle be formed by any means known to the skilled person. The hollow body is preferably formed by a nozzle. The nozzle preferably comprises in the center of its opening a device for drawing off the glass melt as it is formed. The hollow body can be formed, for example, from the glass melt.
[0526] The hollow body can be formed by post-treatment using a nozzle. Suitable post-treatments are in principle any and all processes known to those skilled in the art for producing hollow bodies with solid bodies, such as ramming ducts, drilling, honing or grinding. A particularly preferred post-treatment is passing the solid body over one or more mandrels, thereby forming the hollow body. The mandrels can also be inserted into the solid body to form the hollow body. The hollow body is preferably cooled after it has been formed.
[0527] Once formed, the hollow body is preferably cooled to a temperature below 500°C, for example below 200°C or below 100°C or below 50°C, particularly preferably to a temperature in the range of 20-30°C.
[0528] A second subject of the invention is a quartz glass body obtainable by one of the methods described in the first subject. Correspondingly, processes for producing a quartz body are also known in which steps i.) to vii.) are first carried out.
[0529] In one embodiment, the quartz glass body in one embodiment, the quartz glass body of the second problem, like the quartz glass body obtainable according to the first problem, has at least one, preferably two or more to all of the following characteristics: A] Chlorine content less than 60 ppm; B] aluminum content less than 200 ppb; C]5×10 19 / cm 3 Less than, for example, 0.1 x 10 15 ~3×10 15 / cm 3In particular, the range of 0.5×10 15 ~2.0×10 15 / cm 3 ODC content in the range of; D] content of atoms other than Si, O, H, and C less than 5 ppm; E]log 10 (η(1250℃) / dPas)=11.4~log 10 (η(1250℃) / dPas)=12.9, or log 10 (η(1300℃) / dPas)=11.1~log 10 (η(1300℃) / dPas)=12.2, or log 10 (η(1350℃) / dPas)=10.5~log 10 Viscosity in the range of (η(1350 °C) / dPas) = 11.5 (p = 1013 hPa); F]10 -4 Refractive index homogeneity of less than ; G] cylindrical; H] tungsten content less than 100 ppb, less than 40 ppb, or less than 10 ppb, or less than 5 ppb; I] A molybdenum content of less than 100 ppb, less than 40 ppb, or less than 10 ppb, or less than 5 ppb, where both ppb and ppm are based on the total weight of the quartz glass body at any one time.
[0530] A third object of the present invention is a process for making a light guard comprising the steps of: A / Providing a quartz glass body according to the second subject of the invention or one of its embodiments or a quartz glass body according to the process according to the first subject of the process, in particular by carrying out process steps i.) to vii.) according to the first subject, A quartz glass body is first processed to provide a hollow body having at least one opening; B / inserting one or more core rods into the quartz glass body through at least one opening while maintaining the precursor; C / hot drawing on the precursor from step B / to obtain a light guide having one or more cores and a jacket M1.
[0531] Step A / The quartz glass body provided in step A / is preferably characterized by the properties of the first and second objects of the present invention. This quartz glass body can be obtained in particular by carrying out the process steps i.) to vii.) according to the first object of the present invention. The quartz glass body can also be reshaped to give a hollow body having at least one opening. The quartz glass body thus obtained also has the properties according to the fifth object.
[0532] Step B / One or more core rods are inserted through at least one opening of the quartz glass body (step B / ). In the context of the present invention, a core rod means an object that is provided in a jacket, for example an M1 jacket, and is processed into a light guide. The core rod has a core of quartz glass. The core rod preferably includes a core of quartz glass and a core that surrounds a first jacket layer M0.
[0533] Each core rod has a shape selected to fit the quartz glass body. The outer shape of the core rod preferably corresponds to the shape of the opening of the quartz glass body. Particularly preferably, the quartz glass body is a tube and the core rod is a rod with a circular cross section.
[0534] The diameter of the core rod is smaller than the inner diameter of the hollow body, preferably 0.1 to 3 mm smaller, for example 0.3 to 2.5 mm smaller, or 0.5 to 2 mm smaller, or 0.7 to 1.5 mm smaller, particularly preferably 0.8 to 1.2 mm smaller than the inner diameter of the hollow body.
[0535] The ratio of the inner diameter of the quartz glass body to the diameter of the core rod is preferably in the range of 2:1 to 1.0001:1, for example in the range of 1.8:1 to 1.01:1, or in the range of 1.6:1 to 1.005:1, or in the range of 1.4:1 to 1.01:1, in particular in the range of 1.2:1 to 1.05:1.
[0536] The inner region of the quartz glass body that is not filled by the core rod is preferably filled with at least one further component, such as silicon dioxide powder or silicon dioxide granules.
[0537] It is also possible for the core rod in the quartz glass body to be inserted into at least one additional quartz glass body, the additional quartz glass body having an outer diameter smaller than the inner diameter of the quartz glass body. The core rod inserted into the quartz glass body may already be in two or more additional quartz glass bodies, for example, three or four or five or six or more additional quartz glass bodies.
[0538] The quartz glass bodies that can be obtained in this way using one or more quartz glass bodies are referred to below as "precursors".
[0539] Step C / The precursor is hot drawn (step C / ). The product thus obtained is a light guide having one or more cores and at least one jacket M1.
[0540] The precursor is preferably stretched at a speed in the range of 1 to 100 m / h, for example, at a speed in the range of 2 to 50 m / h or 3 to 30 m / h. Particularly preferably, the quartz glass body is stretched at a speed in the range of 5 to 25 m / h.
[0541] The stretching is preferably carried out at a temperature of up to 2500°C, for example at a temperature in the range of 1700 to 2400°C, particularly preferably at a temperature in the range of 2100 to 2300°C.
[0542] The precursor is preferably conducted through a furnace which heats the precursor externally.
[0543] The precursor is preferably stretched or "elongated" until the desired thickness of the light guide is achieved. The precursor is preferably elongated 1,000 to 6,000,000 times its length, for example 10,000 to 500,000 times its length, or 30,000 to 200,000 times its length, based on the length of the quartz glass body provided in step A / . Particularly preferably, the precursor is elongated to 100,000 to 10,000,000 times its length, for example 150,000 to 5,800,000 times its length, or 160,000 to 640,000 times its length, or 1,440,000 to 5,760,000 times its length, or 1,440,000 to 2,560,000 times its length, based on the length of the quartz glass body in step A / .
[0544] The diameter of the precursor is preferably reduced by elongating the precursor by a factor in the range of 100 to 3,500, for example 300 to 3,000 or 400 to 800 or 1,200 to 2,400 or 1,200 to 1,600, based in each case on the diameter of the quartz glass body provided in step A / .
[0545] A light guide, also called an optical waveguide, may include any material suitable for guiding or directing electromagnetic radiation, particularly light.
[0546] Guiding or directing radiation means extending the radiation over the longitudinal extension of the light guide without essentially impeding or attenuating the intensity of the radiation, the radiation being input to the light guide via one end thereof. The light guide preferably guides electromagnetic radiation in the wavelength range of 170-5000 nm. Preferably, the light guide attenuates radiation in the wavelength range of 0.1-10 dB / km in each case. The light guide preferably has a transmission rate of up to 50 Tbit / s.
[0547] The light guide preferably has a curl parameter of more than 6 m. In the present context, curl parameter is taken to mean the bending radius of the light guide or jacket M1 fixed to the fiber, e.g. the fiber being free to move without the action of external forces.
[0548] The light guide is preferably designed to be bendable. In the sense of the present invention, "bendable" means that the light guide is characterized by a bending radius of 20 mm or less, for example 10 mm or less, particularly preferably 5 mm or less. The bending radius means the narrowest radius that can be formed without breaking the light guide and without affecting the light guide's ability to guide radiation. "Affect" means that bending the light guide attenuates the guided light by more than 0.1 dB. The attenuation is preferably indicated with a reference wavelength of 1550 nm.
[0549] The light guide preferably has an elongated shape. The shape of the light guide is defined by its longitudinal extension L and its cross section Q. The light guide preferably has a rounded outer wall along its longitudinal extension L. The cross section Q of the light guide is always defined in a plane perpendicular to the outer wall of the light guide. If the light guide is doglegged in its longitudinal direction L, the cross section Q is determined perpendicular to a tangent at a point on the outer wall of the light guide. The light guide preferably has a diameter d in the range of 0.04 to 1.5 mm. L The light guide preferably has a length in the range of 1 m to 100 km.
[0550] The light guide can have one or more cores, for example one core or two cores or three cores or four cores or five cores or six cores or seven cores or more than seven cores, particularly preferably one core. More than 90%, for example more than 95%, particularly preferably more than 98% of the electromagnetic radiation guided through the light guide is guided in the core. The light is transported in the core in one of the "preferred" wavelength ranges already mentioned for the light guide. The material of the core is preferably selected from the group consisting of glass or quartz glass or a combination of both, particularly preferably quartz glass. The cores can be made of the same material or different materials, independently of each other. All cores are preferably made of the same material, particularly preferably quartz glass.
[0551] Each core preferably has a circular cross section Q K and has a length L K The cross section of the core Q K is the cross section Q of any further core K It is independent of the cross section Q of the core. K may be the same or different. The cross sections Q of all the cores K are preferably the same. K is always determined in a plane perpendicular to the outer wall of the core and / or the light guide. If the core is doglegged in its longitudinal extension, the cross section Q K is determined perpendicular to the tangent at a point on the outer wall of the core. The length of the core, L K is the length of each further core L K It is independent of the core length L K may be the same or different. The lengths L of all the cores K Each core has a length L preferably in the range of 1 m to 100 km. K Each core has a diameter d K The diameter of one core is d K is the diameter of each further core d K It is independent of the core diameter d K may be the same or different. The diameters d of all the coresK are preferably the same. K is in the range of 0.1 to 1000 μm, for example, 0.2 to 100 μm or 0.5 to 50 μm, and particularly preferably 1 to 30 μm.
[0552] Each core has at least one refractive index that extends perpendicular to the maximum core elongation. The term "refractive index variation" means that the refractive index is constant or varies perpendicular to the maximum core elongation. A preferred refractive index profile corresponds to a concentric refractive index profile, for example, where there is a first range with a maximum refractive index in the center of the core connected by a further range with a lower refractive index. Each core is preferably 100 nm long, 100 nm thick, and 100 nm thick. K The refractive index profile of the core is independent of the refractive index profile of each further core. The refractive index distributions of the cores may be the same or different. The refractive index profile of all cores is preferably the same. In principle, it is also possible for the core to have multiple paths of different refractive index.
[0553] Each refractive index extending perpendicular to the maximum core extension is the maximum refractive index n K Each refractive index extending perpendicular to the maximum core extension may have a lower refractive index. The minimum refractive index of the refractive index profile is preferably less than the maximum refractive index n K The minimum refractive index of the refractive index profile is not more than 0.5 less than the maximum refractive index of the refractive index profile, n K is preferably 0.0001 to 0.15, for example 0.0002 to 0.1, and particularly preferably 0.0003 to 0.05 smaller than the above.
[0554] The core preferably has a refractive index n in the range of 1.40 to 1.60, for example in the range of 1.41 to 1.59, particularly preferably in the range of 1.42 to 1.58. K which has a reference wavelength λ r= 589 nm (sodium D line), at 20 °C and standard pressure p = 1013 hPa (see Test Methods section for details). The refractive index of the core, n K is the refractive index of each further core, n K It is independent of the refractive index of the core, n K The refractive indices n of all the cores can be the same or different. K are preferably equal.
[0555] Each core of the light guide preferably has a density of 1.9 to 2.5 g / cm 3 range, e.g. 2.0-2.4g / cm 3 in the range of 2.1 to 2.3 g / cm 3 The cores preferably have a residual moisture of less than 100 ppb, for example less than 20 ppb or less than 5 ppb, particularly preferably less than 1 ppb, in each case based on the total weight of the cores. The density of the cores is independent of the density of each further core. The densities of the cores may be equal or different. The densities of all cores are preferably equal.
[0556] Where the light guide has more than one core, each core has the above properties independent of further cores, preferably all cores have the same properties.
[0557] According to the invention, the core is surrounded by at least one jacket M1. The jacket M1 surrounds the core, preferably over its entire length. The jacket M1 preferably surrounds at least 95%, for example at least 98% or at least 99%, particularly preferably 100%, of the outer surface, i.e. the entire outer wall of the core. The jacket M1 preferably completely surrounds the cores up to their ends (the last 1-5 cm of each). This serves to protect the core from mechanical influences.
[0558] The jacket M1 is the cross section of the core Q K The core Q may include any material containing silicon dioxide having a lower refractive index than point P on the way to the core Q. KPreferably, the core has at least one point in the middle of the cross section Q of the core, the point being in the center of the core. K Point P on the way has refractive index n Kmax The jacket M1 preferably has a maximum value of the refractive index n K A refractive index n that is at least 0.0001 smaller than M1 The jacket M1 preferably has a refractive index n K The refractive index n is in the range of 0.0001 to 0.5 smaller than the refractive index n M1 has.
[0559] The jacket M1 preferably has a refractive index n in the range of 0.9 to 1.599, for example in the range of 1.30 to 1.59, particularly preferably in the range of 1.40 to 1.57. M1 The jacket M1 preferably has a constant refractive index n M1 The region of constant refractive index is defined as the average refractive index within the region, n M1 is interpreted to mean the area that does not vary by more than 0.0001 from
[0560] The light guide can in principle also comprise further jackets, at least one of which, preferably two or more of them or all of which particularly preferably have a refractive index n K The light guide preferably has one, two, three, four or more jackets surrounding the jacket M1. The further jackets surrounding the jacket M1 preferably have a refractive index smaller than the refractive index n M1 has a refractive index smaller than
[0561] The light guide preferably has one or two or three or four or more further jackets surrounding the core and surrounded by the jacket M1, i.e. located between the core and the jacket M1. More preferably, the further jackets between the core and the jacket M1 have a refractive index n M1 has a refractive index greater than
[0562] The refractive index of the core of the light guide preferably decreases towards the outermost jacket. The refractive index can decrease stepwise or steadily from the core to the outermost jacket. The refractive index can decrease in different sections. More preferably, the refractive index can decrease stepwise in at least one section and steadily in at least one other section. The steps can be of the same height or of different heights. It is quite possible to provide a section of decreasing refractive index between sections of increasing refractive index.
[0563] The different refractive indices of the different jackets may be set by doping the jacket M1, the further jackets and / or the core.
[0564] Depending on how it is made, the core may already have a first jacket layer M0 when it is made. This jacket layer directly adjacent to the core is sometimes called the integral jacket layer. The jacket layer M0 is located closer to the center point of the core than the jacket M1 and any further jackets, if present. The jacket layer M0 does not usually function to guide light and / or radiation. Rather, the jacket layer M0 serves to ensure that radiation remains and is transported within the core, and thus radiation guided in the core is preferably reflected at the transition from the core to the jacket layer M0. This transition from the core to the jacket layer M0 is preferably characterized by a change in refractive index. The refractive index of the jacket layer M0 is preferably smaller than the refractive index n of the core. KThe jacket layer M0 preferably comprises the same material as the core, but is doped or contains an additive so that it has a lower refractive index than the core.
[0565] Preferably, at least the jacket M1 comprises silicon dioxide and preferably has one or more or all of the following characteristics: a) an OH content of less than 5 ppm, particularly preferably less than 1 ppm; b) a chlorine content of less than 200 ppm, preferably less than 100 ppm, for example less than 80 ppm, particularly preferably less than 60 ppm; c) an aluminum content of less than 200 ppb, preferably less than 100 ppb, for example less than 80 ppb, particularly preferably less than 60 ppb; d) 5 × 10 15 / cm 3 Less than, for example, 0.1 x 10 15 ~3×10 15 / cm 3 In particular, the range of 0.5×10 15 ~2.0×10 15 / cm 3 ODC content in the range of; e) a metal content of metals other than aluminum of less than 1 ppm, for example less than 0.5 ppm, particularly preferably less than 0.1 ppm; f)log 10 (η(1250℃) / dPas)=11.4~log 10 (η(1250℃) / dPas)=12.9, or log 10 (η(1300℃) / dPas)=11.1~log 10 (η(1300℃) / dPas)=12.2, or log 10 (η(1350℃) / dPas)=10.5~log 10 Viscosity in the range of (η(1350 °C) / dPas) = 11.5 (p = 1013 hPa); g) curl parameters greater than 6m; h) 1×10 -4 Refractive index homogeneity of less than ; i) a transformation point Tg in the range of 1150 to 1250 ° C, particularly preferably in the range of 1180 to 1220 ° C; Here, ppb and ppm are in each case based on the total weight of the jacket M1.
[0566] The jacket is preferably 1 x 10 -4 The refractive index homogeneity is less than 1 / 1000. The refractive index homogeneity refers to the maximum variation of the refractive index at each point in the sample, for example the jacket M1 or the quartz gas volume, based on the average of all the refractive indices of all the samples determined in the sample. The average is calculated using the refractive indices of at least seven measurement points.
[0567] The jacket M1 preferably has a metal content of metals other than aluminum of less than 1000 ppb, for example less than 500 ppb, particularly preferably less than 100 ppb, in each case based on the total weight of the jacket M1. However, the jacket M1 often has a content of metals other than aluminum in an amount of at least 1 ppb. Such metals are, for example, sodium, lithium, potassium, magnesium, calcium, strontium, germanium, copper, molybdenum, titanium, iron and chromium. These may be present, for example, as elements, as ions or as part of molecules or ions or complexes.
[0568] The jacket M1 can contain further components. The jacket M1 preferably contains less than 5 ppm, for example less than 4.5 ppm, particularly preferably less than 4 ppm, of further components, where ppm is in each case based on the total weight of the jacket M1. The further elements can contain, for example, carbon, fluorine, iodine, bromine and phosphorus. These may be present, for example, as elements, as ions or as part of molecules or ions or complexes. However, the jacket M1 often has a content of atoms other than Si, O, H, C, Cl in an amount of at least 1 ppb.
[0569] The jacket M1 preferably has a carbon content of less than 5 ppm, for example less than 4 ppm or less than 3 ppm, particularly preferably less than 2 ppm, in each case based on the total weight of the jacket M1, but the jacket M1 preferably contains at least 1 ppb of carbon.
[0570] The jacket M1 preferably contains in each case homogeneously distributed amounts of OH, Cl and / or Al.
[0571] In one embodiment of the light guide, the jacket M1 has a weight fraction of at least 80% by weight, for example at least 85% by weight, particularly preferably at least 90% by weight, in each case based on the total weight of the jacket M1 and the core. The jacket M1 preferably has a weight fraction of at least 80% by weight, for example at least 85% by weight, particularly preferably at least 90% by weight, in each case based on the total weight of the jacket M1, the core and further jackets located between the jacket M1 and the core. The jacket M1 preferably has a weight fraction of at least 80% by weight, for example at least 85% by weight, particularly preferably at least 90% by weight, in each case based on the total weight of the light guide.
[0572] The jacket M1 is preferably 2.1 to 2.3 g / cm 3 In particular, the range of 2.18 to 2.22 g / cm 3 It has a density in the range of
[0573] A further aspect relates to a light guide obtainable by a process comprising the following steps: A / Providing a quartz glass body according to the third subject of the present invention or a quartz glass body obtainable by the process according to the first subject, wherein the quartz glass body is first processed into a hollow body having at least one opening; B / Inserting one or more core rods into the quartz glass body through at least one opening to obtain a precursor; C / heat drawing the precursor from step B / to obtain a light guide having one or more cores and a jacket M1.
[0574] Steps A / , B / and C / are preferably characterized by the properties described in the fourth subject matter.
[0575] The light guide is preferably characterised by the properties described in relation to the third subject matter.
[0576] A fourth object of the present invention relates to a process for producing a phosphor comprising the following steps: (i) providing a quartz glass body according to the second subject of the invention or a quartz glass body obtainable by the process according to the first subject, in particular by carrying out the process steps i.) to vii.) according to the first subject, in which the quartz glass body is first processed to obtain a hollow body; (ii) optionally attaching electrodes to the hollow body; (iii) filling the hollow body with a gas;
[0577] Step (i) The quartz glass body is provided in step (i). The quartz glass body provided in step (i) is first processed to obtain a hollow body comprising at least one opening, for example one opening or two openings or three openings or four openings, particularly preferably one opening or two openings.
[0578] A quartz glass body obtainable according to the method according to the first subject is preferably provided for step (i). The quartz glass body preferably has the properties described in the course of the first or second subject.
[0579] There are two or more options that can be considered for processing the quartz glass body according to the fourth problem.
[0580] The processing of the quartz glass body into a hollow body with one opening can in principle be carried out by any and all processes known to those skilled in the art that are suitable for producing a hollow glass body with one opening. Suitable processes include, for example, pressing, blowing, suction or a combination thereof. It is also possible to form a hollow body with one opening, for example by closing one opening to fuse together.
[0581] The hollow body preferably comprises a material containing silicon dioxide in an amount in the range from 98 to 100 wt.-%, for example in the range from 99.9 to 100 wt.-%, particularly preferably up to 100 wt.-%, in each case based on the total weight of the hollow body.
[0582] The material from which the hollow body is made preferably has at least one, preferably more than one, preferably two or preferably all of the following properties: HK1. A silicon dioxide content of preferably more than 95 wt.-%, for example more than 97 wt.-%, particularly preferably more than 99 wt.-%, based on the total weight of the material; HK2.2.1~2.3g / cm 3 In particular, the range of 2.18 to 2.22 g / cm 3 Density in the range of; HK3. Translucency at at least one wavelength in the visible range from 350 to 750 nm in the range of 10 to 100%, for example in the range of 30 to 99.99%, particularly preferably in the range of 50 to 99.9%, based on the amount of light generated in the hollow body; HK4. OH content of less than 500 ppm, for example less than 400 ppm, particularly preferably less than 300 ppm; HK5. Chlorine content of less than 200 ppm, preferably less than 100 ppm, for example less than 80 ppm, particularly preferably less than 60 ppm; HK6. Aluminum content of less than 200 ppb, for example less than 100 ppb, particularly preferably less than 80 ppb; HK carbon content of less than 7.5 ppm, for example less than 4.5 ppm, particularly preferably less than 4 ppm; HK8.5×1019 / cm 3 Less than ODC content; HK 9. A metal content of metals other than aluminum of less than 1 ppm, for example less than 0.5 ppm, particularly preferably less than 0.1 ppm; HK10.log 10 η(1250℃)=11.4~log 10 η(1250°C)=12.4 and / or log 10 η(1300℃)=11.1~log 10 η(1350°C)=11.7 and / or log 10 η(1350℃)=10.5~log 10 Viscosity in the range of η(1350 °C) = 11.1 (p = 1013 hPa); HK11.1 Transformation point Tg in the range of 1150 to 1250 ° C, particularly preferably in the range of 1180 to 1220 ° C; Here, ppm and ppb are in each case based on the total mass of the hollow body.
[0583] Step (ii) Prior to filling with gas, the hollow body from step (i) is fitted with an electrode, preferably two electrodes. The electrodes are preferably connected to a power supply. The electrodes are preferably connected to a lamp stand.
[0584] The electrode material is preferably selected from the group of metals. In principle, any metal that is not oxidized, corroded, melted or otherwise affected can be selected as the electrode material. The electrode material is preferably selected from the group consisting of iron, molybdenum, copper, tungsten, rhenium, gold and platinum, or at least two of them, with tungsten, molybdenum or rhenium being preferred.
[0585] Step (iii) The hollow body provided in step (i) and optionally fitted with electrodes in step (ii) is filled with a gas.
[0586] The filling can be carried out by any and all processes known to the person skilled in the art that are suitable for filling. The gas is preferably supplied to the hollow body by means of at least one opening.
[0587] The hollow body is preferably evacuated before filling with gas, preferably to a pressure of less than 2 mbar. Gas is then injected to fill the hollow body with gas. These steps can be repeated to minimize contamination with air, especially oxygen. These steps are preferably repeated at least twice, for example at least three times or at least four times, particularly preferably at least five times, until the amount of contamination with other gases such as air, especially air, is sufficiently low. This approach is particularly preferred for filling hollow bodies with openings.
[0588] If the hollow body has two or more openings, the hollow body is preferably filled through one of the openings. Air present in the hollow body before it is filled with gas can escape through at least one further opening. The gas passes through the hollow body until the amount of contamination by other gases, in particular oxygen, is sufficiently low.
[0589] The hollow body is preferably filled with an inert gas or a combination of two or more inert gases, such as nitrogen, helium, neon, argon, krypton, xenon or a combination of two or more thereof, particularly preferably krypton, xenon or a combination of nitrogen and argon. Further preferred filling agents for the hollow body of the luminous body are deuterium and mercury.
[0590] Once filled, the hollow body is preferably gas-tight so that gas cannot escape during further processing and / or air cannot enter from the outside during further processing. The sealing may be performed by melting or by applying a seal. Suitable seals are, for example, quartz glass seals or lamp stands that are melted onto the hollow body. The hollow body is preferably closed by melting.
[0591] The light emitter comprises a hollow body and, optionally, electrodes. The light emitter preferably has at least one, for example at least two or at least three or at least four, in particular at least five, of the following properties: I.) 0.1cm 3 ~10m 3 range, e.g. 0.3cm 3 ~8m 3 In particular, 0.5 cm 3 ~5m 3 Volume in the range of; II.) A length in the range of 1 mm to 100 m, for example in the range of 3 mm to 80 m, particularly preferably in the range of 5 mm to 50 m; III.) A release angle in the range of 2 to 360°, for example in the range of 10 to 360°, particularly preferably in the range of 30 to 360°; IV.) Emission in the wavelength range of 145 nm to 4000 nm, for example in the range of 150 nm to 450 nm or 800 nm to 4000 nm, particularly preferably in the range of 160 nm to 280 nm; V.) Power in the range of 1 mW to 100 kW, particularly preferably in the range of 1 kW to 100 kW or in the range of 1 to 100 watts.
[0592] A further aspect relates to a light emitter obtainable by a method comprising the steps of: (i) a step for preparing a quartz glass body according to the second object of the present invention or obtainable according to the first object of the present invention, in particular by carrying out the process steps i.) to vii.), in which the quartz glass body is first processed into a hollow body; (ii) optionally attaching electrodes to the hollow body; (iii) filling the hollow body with a gas;
[0593] Steps (i), (ii) and (iii) are preferably characterised by the properties described in the course of the seventh task.
[0594] The luminescent body is preferably characterized by the properties described in the course of the seventh task.
[0595] A fifth object of the present invention relates to a process for producing a shaped body comprising the following steps: (1) Providing a quartz glass body according to the second subject of the present invention or according to the first subject, in particular obtainable by carrying out the process steps i.) to vii.) according to the first subject; (2) A step of forming the quartz glass body to obtain a formed body.
[0596] The quartz glass body provided in step 1) is a quartz glass body according to the second subject of the present invention or a quartz glass body obtainable by the method according to the first subject of the present invention. The provided quartz glass body preferably has the properties of the first or second subject.
[0597] Step (2) To form the quartz glass body provided in step (1), any and all processes known to those skilled in the art and suitable for forming quartz glass may be considered. The quartz glass body is preferably made into a shaped body as described in the first, fourth and fifth tasks. The shaped body may further preferably be formed by a method known to glass blowers.
[0598] The shaped bodies can in principle take any form that can be formed from quartz glass. Preferred shaped bodies are, for example: - hollow bodies with at least one opening, such as circular pistons and upright pistons; - attachments and closures for such hollow bodies, -Open products such as shells and boats (or wafer carrier frames), - Crucibles available in both open and lock designs; -metal sheets and windows, -cuvette, Tubes and hollow cylinders, e.g. reaction tubes, profile tubes, rectangular chambers, - for example bars, rods and blocks, of round or angular, symmetrical or asymmetrical design; - Tubes and hollow cylinders sealed on one or both sides, - Dome and bell, - flanges, - lenses and prisms, - Welding parts, - Curved parts, e.g. convex or concave surfaces and metal sheets, curved rods and tubes.
[0599] According to one embodiment, the shaped body may be treated after formation. In principle, all methods described in the course of the first task that are suitable for finishing quartz glass bodies may be considered here. The shaped body may be preferably mechanically processed, for example by drilling, honing, external grinding, crushing or elongation.
[0600] A further aspect relates to a shaped body obtainable by a process comprising the steps of: (1) Providing a quartz glass body according to the second subject of the present invention or a quartz glass body obtainable by the method according to the first subject of the present invention, in particular by carrying out the process steps i.) to vii.) according to the first subject; (2) A step of forming the quartz glass body to obtain a formed body.
[0601] Steps (1) and (2) are preferably characterized by the properties described in the course of the eighth task.
[0602] The shaped body is preferably characterized by the properties described in the course of the eighth task.
[0603] A sixth object of the present invention is a method for producing a coating on a substrate, the method comprising the steps of: |A| Providing a silicon dioxide suspension and a base obtainable according to the first task or one of its embodiments; |B| applying a coating of a silicon dioxide suspension to a substrate, A coating is formed on the substrate.
[0604] The silicon dioxide suspension provided in step |A| can be obtained by the process according to the first subject of the present invention. The silicon dioxide suspension can have further properties corresponding to the embodiments described in connection with the embodiments described in the first subject of the present invention.
[0605] The application in step B can in principle be carried out by any process suitable for producing a coating, with at least a portion of the substrate being coated with the silicon dioxide suspension.
[0606] In further embodiments, application can be by depositing the silicon dioxide suspension on the substrate, or by immersing the substrate in the silicon dioxide suspension, or a combination of both forms. Application by deposition of the silicon dioxide suspension is carried out, for example, by spin coating, infiltration, casting, dripping, pouring, spraying, raking, coating, or by printing, for example via a metering pump or inkjet, silk screen, intaglio, offset or buffer printing, on the substrate. The silicon dioxide suspension can be applied at a wet film thickness in the range of 0.01 μm to 250 μm, for example in the range of 0.1 μm to 50 μm.
[0607] Deposition is further understood to mean that the silicon dioxide suspension used is applied to the substrate via any convenient means. This can be done by different convenient means. Thus, the silicon dioxide suspension applied to the substrate can be sprayed through a nozzle or injected or deposited through a slit nozzle. Other suitable methods are curtain casting and spin coating. The silicon dioxide suspension can also be applied to the surface of the substrate, for example, via a roll or roller. Known spraying and / or injection processes are, for example, microdosing or digital printing through a nozzle. This can be done using the silicon dioxide suspension used for deposition, or the silicon dioxide suspension is simply dripped onto the substrate.
[0608] In the case of immersion, the substrate can be drawn through a bath in the silicon dioxide suspension. If the substrate is only partially coated, only the surface to be coated in the silicon dioxide suspension can be immersed and, if necessary, drawn out again, which is carried out, for example, in dip coating. To achieve different coating thicknesses, immersion can be used repeatedly. The coating thickness can also be set by the viscosity and solids content of the silicon dioxide suspension. A wet layer thickness of the silicon dioxide suspension can thus be achieved by applying the silicon dioxide suspension in the range of 0.5 to 1000 μm, preferably in the range of 5 to 250 μm, particularly preferably in the range of 10 to 100 μm.
[0609] This is optionally, but not necessarily, followed by a step [C] of reducing the liquid content of the coating. Step |C| is carried out until the liquid content of the coating reaches or falls below a set point, based on the total weight of the coating. This set point may be, for example, 10%, 5%, 2% or 0.2% by weight, where the weight percentage is in each case based on the total weight of the coating. In principle, any and all methods known to the skilled person that may be suitable for reducing the liquid content of the layer can be considered, in particular at least one selected from the group consisting of heating and drying, drying by covering the coating with a gas or a gas mixture, evaporating the liquid at reduced ambient pressure, exciting the molecular motion of the liquid with microwaves, for example in the case of water, etc. A combination of two or more of the methods can also be considered, which combinations can be designed to be spatially and / or temporally simultaneous, spatially and / or temporally consecutive or spatially and / or temporally overlapping. In this context, overlapping means that one method can be started even before the preceding method is completed.
[0610] The invention will now be described with reference to the drawings, which are not to scale and are not intended to limit the invention. [Brief description of the drawings]
[0611] [Figure 1] FIG. 1 is a diagram showing a flow chart (a method for producing a quartz glass body). [Diagram 2] FIG. 2 is a diagram showing a modified example of the flow chart (method of producing a quartz glass body). [Diagram 3] FIG. 3 shows a first filter arrangement having three filter stages: a first, a second and a third filter stage. [Figure 4] FIG. 4 shows a schematic diagram of a spray tower. [Diagram 5] FIG. 5 shows a schematic diagram of a hanging crucible in a furnace. [Figure 6] FIG. 6 shows a schematic diagram of a stationary crucible in a furnace. [Figure 7] FIG. 7 shows a schematic diagram of a crucible equipped with a dew point measuring device. [Figure 8] FIG. 8 is a flowchart (a method for producing a molded body). [Figure 9] FIG. 9 shows an exemplary representation a) of the particle size distribution in the slurry before step iii.), b) of the precursor suspension after dispersion in step iii.). [Figure 10] FIG. 10 shows examples of high-temperature quartz glass bodies: a) many bubbles, b) few bubbles, and c) very many bubbles (foam glass). [Figure 11] FIG. 11 shows a comparison of tungsten contamination in quartz glass samples: a) hot glass body, a) heavily contaminated with tungsten, b) no tungsten contamination, c) tungsten discoloration on frozen twin glass tube. [Figure 12] FIG. 12 shows a comparison of frozen quartz glass samples in which the melt was formed from granulation made from a) unfiltered silicon dioxide suspension; b) filtered silicon dioxide suspension according to the invention. [Figure 13] FIG. 13 shows a schematic diagram of the setup for evaluating the fluorescence of a fused silica sample. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0612] FIG. 1 shows a flow chart including steps 101-107 of a method 100 for making a quartz glass body according to the present invention, which includes at least the following steps: (i) providing a powder of silicon dioxide particles and a liquid 101; (ii) providing a slurry by mixing the powder with a liquid; (iii) treating the slurry with ultrasound 103 to obtain a precursor suspension; (iv) passing at least a portion of the precursor suspension through a first multi-stage filter device (104) from which a silicon dioxide suspension is obtained; v.) forming silicon dioxide granules from the silicon dioxide suspension; vi.) forming a glass melt from the silicon dioxide granules in a furnace; vii.) forming a quartz glass body from at least a portion of the glass melt.
[0613] The processing of the slurry in step iii.) involves grinding at least a portion of the silicon dioxide particles to obtain a so-called precursor suspension. The first multi-stage filter device in step iv.) is designed to have at least a first, a second and a third filter stage, the second filter stage being downstream of the first filter stage and the third filter stage being downstream of the second filter stage. Each filter stage comprises at least one filter. Step v.) involves granulation, where the silicon dioxide granules have a larger particle size than the silicon dioxide particles contained in the silicon dioxide particles. In the method described in FIG. 1, silicon components other than silicon dioxide are added in at least one of the process steps (not shown).
[0614] The furnace includes a melting furnace, which can be designed as both a suspended and a stationary melting furnace (see figures 5 and 6). The furnace and / or the melting crucible also have at least one gas outlet, but generally also a gas inlet, by means of which the atmosphere present in the furnace can be influenced. For a detailed description of this, and in particular of the process when measuring the dew point of the gas as it leaves the furnace, see figures 5, 6 and 7.
[0615] The melting in step 106 is preferably carried out in a reducing hydrogen atmosphere. In step 107, a quartz glass body is formed. Here, the formation of the quartz glass body is preferably carried out by removing at least a part of the glass melt from the crucible and cooling it. It can be removed through a nozzle at the lower end of the crucible. In this case, the shape of the quartz glass body can be determined by the design of the nozzle. For example, a solid body can be obtained. A hollow body is obtained, for example, when a mandrel is also provided in the nozzle. This method for producing a quartz glass body shown by way of example, in particular step 107, is preferably carried out continuously. As an alternative to step 107, a solid quartz glass body can be formed in an optional downstream step 108.
[0616] Figure 2 shows the same method as in Figure 1. A silicon component 210 other than silicon dioxide is added during step i.) 201, ii.) 202 or step v.) 205, in the latter case preferably before forming the granules. The silicon component 210 can also be added during two or all three steps, i.e. in more than one portion.
[0617] Figure 3 shows a schematic filter arrangement including three filter stages, each having a first filter 301, a second filter 302 and a third filter 303, which are arranged downstream.
[0618] FIG. 4 shows a preferred embodiment of a spray tower 1100 for spray granulation of silicon dioxide. The spray tower 1100 includes a feed 1101 through which a pressurized slurry containing silicon dioxide powder and liquid is fed to the spray tower. At the end of the line is a nozzle 1102 through which the slurry is fed in a fine distribution to the spray tower. The nozzle is preferably oriented at an upward angle so that the slurry is sprayed into the spray tower as fine droplets in the direction of the nozzle device and then falls in a curve driven by gravity. At the top of the spray tower is a gas inlet 1103. Injecting gas through the gas inlet 1103 creates a gas flow opposite to the direction in which the slurry leaves the nozzle 1102. The spray tower 1100 also includes a screening device 1104 and a sieve device 1105. The screening device 1104 sucks in particles smaller than a defined particle size and is removed via an output 1106. The suction strength of the screening device 1104 can be adjusted depending on the particle size of the particles to be sucked. The sieve device 1105 filters particles exceeding a defined particle size, which are removed via the outlet 1107. The sieve permeability of the sieve device 1105 can be selected depending on the particle size of the particles to be sucked. The remaining particles, silicon dioxide granules of the desired particle size, are removed via the outlet 1108.
[0619] FIG. 5 shows a preferred embodiment of a furnace 800 with a hanging crucible. The crucible 801 is arranged suspended in the furnace 800. The crucible 801 has a suspension 802 in its upper region and has a solid inlet 803 and a nozzle 804 as an outlet. The crucible 801 is filled with silicon dioxide granules 805 through the solid inlet 803. During operation, the silicon dioxide granules 805 are present in the upper region of the crucible 801 and the glass melt 806 is present in the lower region of the crucible 801. The crucible 801 can be heated by a heating element 807 arranged outside the crucible wall 810. The furnace also has an insulating layer 809 between the heating element 807 and the outer furnace wall 808. The space between the insulating layer 809 and the crucible wall 810 can be filled with gas and has a gas inlet 811 and a gas outlet 812 for this purpose. The quartz glass body 813 can be removed from the furnace through the nozzle 804.
[0620] FIG. 6 shows a preferred embodiment of a furnace 900 with a stationary crucible. The crucible 901 is erected in the furnace 900. The crucible 901 has a stationary surface 902, a solid inlet 903 and a nozzle 904 as an outlet. The crucible 901 is filled with silicon dioxide granules 905 through the inlet 903. During operation, the silicon dioxide granules 905 are present in the upper region of the crucible 901 and the glass melt 906 is present in the lower region of the crucible 901. The crucible 901 can be heated by a heating element 907 arranged on the outside of the crucible wall 910. The furnace also has an insulating layer 909 between the heating element 907 and the outer furnace wall 908. The space between the insulating layer 909 and the crucible wall 910 can be filled with gas and has a gas inlet 911 and a gas outlet 912 for this purpose. The quartz glass body 913 can be removed from the crucible 901 through the nozzle 904.
[0621] FIG. 7 shows a melting crucible 1400. The crucible has a solid inlet 1401 and an outlet 1402. In operation, silicon dioxide granules 1403 are conically located in the upper region of the crucible 1400, while glass melt 1405 is present in the lower region of the crucible. The crucible 1400 has a gas inlet 1406 and a gas outlet 1407. The gas inlet 1406 and the gas outlet 1407 are arranged above the conical cone 1404 of the silicon dioxide granules 1403. The gas outlet 1407 includes a gas line 1408 and a device 1409 for measuring the dew point of the exiting gas. The device 1409 includes, for example, a dew point level hygrometer (not shown here). The distance between the crucible and the device 1409 for measuring the dew point can vary. The quartz glass body 1410 can be removed through the outlet 1402 of the crucible 1400.
[0622] FIG. 8 shows a flow chart including steps 401 and 402 of a method for making a shaped body. In a first step 401, a quartz glass body is provided, preferably a quartz glass body made as shown in FIG. 1. Such a quartz glass body may be a solid or hollow quartz glass body. From the solid quartz glass body provided in step 401, a shaped body is formed in a second step 402.
[0623] Graph a) of FIG. 9 shows, by way of example, the particle size distribution of a slurry of silicon dioxide powder in water on which the method is based. The graph shows not only the amount of fully slurried silicon dioxide particles with a particle size of less than 1 μm, but also a series of agglomerates in the ranges of 1-5 μm and 10-100 μm. Graph b) shows the particle size distribution of a silicon dioxide suspension obtained by dispersing a silicon dioxide slurry as in graph a). Here, all particles are dispersed. No silicon dioxide particles with a particle size of more than 1 μm were shown. Through subsequent filtration, the particle size distribution from FIG. 5b) of the silicon dioxide particles remains. However, particles other than silicon dioxide are separated.
[0624] FIG. 10 shows comparative images of (hot) glass bodies after removal from the melting furnace by about 1 m, where a) a melt formed from an unfiltered silicon dioxide suspension was used, b) a glass body in which the melt used was a granulation of a filtered silicon dioxide suspension according to the invention, and c) a glass body in which the melt used was a granulation as in Example 15-4, i.e. a suspension of pyrogenic silicic acid was treated in a ball mill (zirconium oxide balls and polyurethane-coated cup) before filtration.
[0625] FIG. 11 shows comparative images of glass bodies containing tungsten contamination. Images a) and b) show a hot glass body after removal from the melting crucible by about 1 m. Image a) shows a glass body contaminated with tungsten, which shows streaks and discoloration. Image b) shows a glass body without tungsten contamination or the like. Image c) shows, as an example, two cooled twin glass tubes. The glass tube on the left is transparent but appears darker. The color tone is due to a relatively homogeneous tungsten contamination. The glass tube on the right does not contain such contamination. It is transparent and non-absorbing in the visible range.
[0626] FIG. 12 shows two different cooled quartz glass bodies. The quartz glass body in image a) was made from a suspension of silicon dioxide particles that was not treated according to the invention. It contains a large amount of larger air bubbles. The quartz glass body in image b) was made based on a silicon dioxide suspension that was treated according to the invention. Almost no air bubbles are visible.
[0627] Figure 13 shows a schematic diagram of the setup for determining the fluorescence of a quartz glass sample. The sample 1301 is illuminated with UV light from a UV lamp 1303 at an angle (α) of 90° to the observer's line of sight 1302 in a dark room in front of a black background. The distance from the UV lamp to the sample is less than 1 cm. The sample has a length of 10 mm in the direction of travel of the UV light.
[0628] Test Method a.OH content The OH content of the glass is determined by infrared spectroscopy using the method described in DM Dodd and DM Raser "Optical Determinations of OH in Fused Silica" (JAP37,3991 (1966)). Instead of the equipment described there, an FTIR (Fourier Transform Infrared Spectrometer, currently System 2000 from Perkin Elmer) is used. In principle, the spectrum is characterized by a peak at about 3670 cm -1 and absorption bands at approximately 7200 cm -1 The bands used are selected based on the rule that the transmission loss due to OH absorption is between 10 and 90%.
[0629] b. Oxygen depletion center (ODC) As a quantitative proof, the ODC(I) absorption at 165 nm is determined by measuring a transmission sample with a thickness of 1-2 mm using a VUVAS 2000 model vacuum UV spectrometer by McPherson, Inc. (USA).
[0630] In this case the following applies:
[0631]
number
[0632] c.Elemental analysis c-1) The solid sample is ground, then about 20 g of the sample is placed in an HF-resistant container, completely covered with HF and heat-treated at 100 ° C for 1 h. Once cooled, the acid is poured off and the sample is washed several times with the purest water. The container is then dried together with the probe in a drying cabinet.
[0633] Approximately 2 g of solid sample (crushed material, washed as above; dust not directly pretreated, etc.) is placed in an HF-resistant rocking vessel and 15 ml of HF (50 wt%) is added. The rocking vessel is locked and the solid sample is heat-treated at 100 °C until it is completely dissolved. The rocking vessel is then opened and further heat-treated at 100 °C until the solution is completely evaporated. Meanwhile, the rocking vessel is filled with 3 × 15 ml of ultrapure water. 1 ml of HNO3 is added to the rocking vessel to dissolve the separated contaminants and the water is filled up to 15 ml with ultrapure water. The test solution is now ready.
[0634] c-2) ICP-MS / ICP-OES measurement The choice of whether to use OES or MS depends on the expected elemental concentration. Typical MS determination thresholds are about 1 ppb for MS and about 10 ppb for OES (based on the amount of sample weighed in each case). It differs slightly for each element. The determination of elemental concentrations with the test equipment is carried out according to the instructions of the equipment manufacturer (ICP-MS: Agilent 7500 ce; ICP-OES: Perkin Elmer 7300 DV) and uses certified standard solutions for calibration. The elemental concentration that the equipment determines in the solution (15 ml) is then extrapolated to the weight of the sample used (2 g).
[0635] NOTE: The acid, container, water and equipment must be pure enough to determine the elemental concentrations to be proven. This is then rechecked by connecting a blind sample that does not contain quartz glass.
[0636] The elements determined by this means are: Li, Na, Mg, K, Ca, Fe, Ni, Cr, Hf, Zr, Ti, V, Nb, W, Mo, Al.
[0637] c-3) Do not prepare a sample as in step c-1), but place 15 ml of the liquid sample in a rocking container and measure the liquid sample as above, without extrapolating to the original amount weighed.
[0638] The exact decision thresholds for ICP-MS and / or ICP-MS depending on the analyzed element are given in the table below:
[0639] [Table 3]
[0640] d. Determining Liquid Density Liquid density is determined by weighing a precisely defined volume of liquid into a test vessel that is inert to the liquid and its components, where the empty weight and the weight of the filled vessel are measured. The density is obtained by dividing the difference between the two weight measurements by the volume of the liquid weighed.
[0641] e. Testing for evidence of fluoride 15 g of quartz glass sample is crushed and treated in nitric acid to clean at a temperature of 70 ° C. The sample is then rinsed several times with ultrapure water and then dried. From this, 2 g of sample is weighed into a nickel crucible and covered with 10 g of Na2CO3 and 0.5 g of ZnO. The crucible is covered with a Ni cover and annealed at 1000 ° C for 1 hour. The nickel crucible is then filled with water and boiled until the melt cake is completely dissolved. The solution is transferred to a 200 ml test tube and filled up to 200 ml with the purest water. After separating the undissolved components, 30 ml is taken and transferred to a 100 ml test tube, 0.75 ml of acetic acid and 60 ml of TISAB are added and filled up with the purest water. The test solution is transferred to a 150 ml glass beaker.
[0642] The fluoride content of the test solution is determined according to the manufacturer's instructions by means of an ion-sensitive (fluoride) electrode and display unit suitable for the expected concentration range, in this case a fluoride ion-selective electrode and reference electrode F-500 with R503 / D for pMX 3000 / pH / ION from Wissenschaftlich-Technische Werkstaetten GmbH. The fluoride concentration in the quartz glass is calculated from the fluoride concentration in the solution, the dilution factor and the weighing.
[0643] f. Chlorine evidence test (≧60ppm) 15 g of glass sample are crushed and cleaned by treatment in nitric acid at about 70 ° C. The sample is then rinsed several times with the purest water and then dried. From this, 2 g of sample are placed in the PTFE insert of a pressure vessel, 15 ml of NaOH (c = 10 mol / l) is added, closed with a PTFE cover and placed in a pressure vessel. This is sealed and treated at about 155 ° C for 24 hours. After cooling, the PTFE insert is removed and the solution is transferred completely to a 100 ml test tube. Now, 10 ml of HNO3 (65 wt%) and 15 ml of acetate buffer are added, allowed to cool and made up to 100 ml with the purest water. The test solution is transferred to a 150 ml glass beaker. The test solution should have a pH value in the range of 5 to 7.
[0644] The determination of the chloride content from the test solutions is carried out according to the manufacturer's instructions with an ion-sensitive (chloride) electrode and display device suitable for the expected concentration range, in this case a type Cl-500 electrode and a type R-503 / D reference electrode for pMX 3000 / pH / ION by Wissenschaftlich-Technische Werkstaetten GmbH.
[0645] g. Chlorine content (<60ppm) The quartz glass chlorine content of <60 ppm to 0.1 ppm is determined by neutron activation analysis (NAA). For this, three borehole samples, each 3 mm in diameter and 1 cm in length, are taken. These are sent to the laboratory to be analyzed, in this case the Institute of Nuclear Chemistry at the Johannes Gutenberg University Mainz. To remove chlorine contaminants from the samples, it is agreed with the laboratory that the samples are thoroughly washed in an HF bath on site and only immediately before the measurements. Each bore is measured several times. The laboratory then sends back the results and the bore.
[0646] h.Optical properties The transmittance from fused silica samples is determined using a commercially available matrix or FTIR spectrometer from Perkin Elmer (Lambda 900 [190-3000 nm] or System 2000 [1000-5000 nm]). The section is guided by the test range required.
[0647] To determine the absolute transmission, the specimen body is polished with parallel planes (surface roughness RMS < 0.5 nm) and, once all residues have been polished off, all residues are removed from the surface by ultrasonic treatment. The thickness of the specimen is 1 cm. If strong transmission losses due to contamination, doping, etc. are expected, thicker or thinner specimens must be selected to stay within the test range of the instrument. The specimen thickness is selected such that the radiation causes artifacts to appear slightly on the specimen (measured length) and at the same time the effect is sufficiently detectable to be measured.
[0648] To measure its opacity, the sample is placed in front of an Ulbricht sphere in the radiation beam. The opacity is calculated using the transmittance value T so measured according to the formula: O=1 / T=I0 / I.
[0649] i. Refractive index and refractive index distribution in the tube or bar The refractive index profile of the rod / bar can be characterized by a York Technology Ltd. Preform Profiler P102 or P104. For this, the rod is inserted into a measurement chamber and the measurement chamber is sealed. The measurement chamber is then filled with an immersion oil with a refractive index at the test wavelength of 633 nm that is very similar to the refractive index at 633 nm through the outermost glass layer. A laser beam is then passed through the test chamber in the radial direction. At the rear (radial direction) of the measurement chamber is mounted a detector that determines the angle of refraction (irradiation into the measurement chamber versus radiation emerging from the measurement chamber). Assuming that the refractive index profile of the rod is symmetrical, the diametrical progression of the refractive index can be reconstructed by the inverse Abel transformation. These calculations are carried out using software from the equipment manufacturer York.
[0650] Similar to the description above, a York Technology Ltd. Preform Profiler P104 is used to determine the refractive index of the sample. Even for an isotropic sample, measuring the refractive index profile will only give a single value for the refractive index.
[0651] j.Carbon content Quantitative measurement of the surface carbon content of silicon dioxide granules and silicon dioxide powder is carried out by oxidizing all surface carbon contaminants (except SiC) with oxygen to carbon dioxide using a RC612 carbon analyzer by Leco Corporation (USA). For this, 4.0 g of sample is weighed, placed in a piece of quartz glass metal sheet and inserted into the carbon analyzer. The sample is flushed with pure oxygen and heated at 900 ° C for 180 seconds. The CO2 formed here is recorded by the infrared detector of the carbon analyzer. The evidence of detection threshold under these measurement conditions is ≦ 1 ppm (ppm by weight) carbon.
[0652] Quartz glass metal sheet pieces suitable for this analysis in the above carbon analyzer are available as consumables for LECO analyzers with LECO No. 781-335, in this case from Deslis Laborhandel, Flurstrasse 21, D-40235 Duesseldorf, Germany, Deslis no. LQ-130XL. Such metal sheet pieces have width / length / height dimensions of approximately 25 mm / 60 mm / 15 mm. The quartz glass metal sheet pieces are filled to half height with the sample material. For silicon dioxide powder, 1.0 g of sample material can be weighed. The lower detection limit is then <1 ppm carbon by weight. On the same quartz glass metal sheet pieces, with the same filling height, up to 4 g of silicon dioxide granulation can be weighed (average particle size in the range of 50-500 μm). The lower detection threshold is then approximately 0.1 ppm carbon by weight. The lower detection threshold is reached when the measured area integral of the sample does not exceed 3 times the measured area integral of the blank sample (blank sample = above process but with an empty piece of quartz glass metal sheet).
[0653] k. Curl parameters The curl parameter (also called "fibre curl") is determined in accordance with DIN EN 60793-1-34:2007-01 (the German version of IEC standard 60793-1-34:2006) and is measured according to the method described in Appendix A, sections A.2.1, A.3.2 and A.4.1 ("Extreme Value Technique").
[0654] l. Attenuation The attenuation is determined in accordance with DIN EN 60793-1-40:2001 (IEC 60793-1-40:2001, German edition) and is measured at a wavelength λ=1550 nm according to the method described in the appendix ("cutback method").
[0655] m. Viscosity of slurries and suspensions The slurry is set to a concentration of 30% solids by weight with demineralized water (Direct-Q 3UV, Millipore, water quality: 18.2 mΩcm). The viscosity is then measured with an Anton-Paar MCR102, measuring the viscosity at 5 revolutions per minute (rpm), at a temperature of 23° C. and an air pressure of 1013 hPa. The procedure for the suspension is exactly the same.
[0656] n. Thixotropy and rheopexy -n1. Thixotropy The slurry or suspension is set to a concentration of 30% solids by weight with demineralized water (Direct-Q 3UV, Millipore, water quality 18.2 mΩcm). The thixotropy is then determined using an Anton-Paar MCR102 with a ball-metal sheet configuration. For this, the viscosity is measured at 5 rpm and at 50 rpm. The quotient of the first and second values gives the thixotropy index. The measurements are taken at a temperature of 23° C.
[0657] -n2.Leopexy The slurry or suspension is set to a concentration of 60 wt.% solids in demineralized water (Direct-Q 3UV, Millipore, water quality 18.2 mΩcm). The viscosity of the slurry and / or suspension is measured at 25° C. with a Kinexus pro+ rheometer equipped with a blade stirrer from Malvern Panalytical Ltd. at a constant shear rate of 25 / s or 100 / s for 15 min.
[0658] o. Zeta potential of the slurry or suspension Zeta potential measurements are performed using a zeta potential test cell (Flow Cell, Beckman Coulter). The sample is dissolved in demineralized water (Direct-Q 3UV, Millipore, water quality 18.2 mΩcm) to obtain a 20 ml solution with a concentration of 1 g / l. The pH is brought to 7 by adding HNO3 solutions with concentrations of 0.1 mol / l and 1 mol / l and NaOH solution with a concentration of 0.1 mol / l, measured at a temperature of 23°C.
[0659] p. The isoelectric point of the slurry or suspension To determine the isoelectric point, a zeta potential test cell (Flow Cell, Beckman Coulter) and an automatic titrator (DelsaNano AT, Beckman Coulter) are used. The sample is dissolved in demineralized water (Direct-Q 3UV, Millipore, water quality 18.2 mΩcm) to obtain a 20 ml solution with a concentration of 1 g / l. The pH is changed by adding HNO3 solutions with concentrations of 0.1 mol / L and 1 mol / l and NaOH solution with a concentration of 0.1 mol / l. The isoelectric point is the pH value at which the zeta potential measured at a temperature of 23°C is equal to 0.
[0660] q. pH value of the slurry or suspension The pH value of the slurry is measured u...
Claims
1. A method for making a quartz glass body, comprising: i.) providing a powder of silicon dioxide particles and a liquid; ii.) mixing the powder with the liquid to form a slurry containing the liquid and the silicon dioxide particles; iii.) treating the slurry with ultrasound to obtain a precursor suspension; iv.) passing at least a portion of said precursor suspension through at least a first multi-stage filter device to obtain a silicon dioxide suspension; v.) forming silicon dioxide granules from the silicon dioxide suspension; vi.) forming a glass melt from the silicon dioxide granules in a furnace; vii.) forming a quartz glass body from at least a portion of the glass melt; The process steps include The treating of the slurry in step iii.) comprises deagglomerating at least a portion of the silicon dioxide particles; A silicon component other than silicon dioxide is added in at least one of the process steps; Step v.) comprises at least granulation, The silicon dioxide granules have a particle size larger than the silicon dioxide particles contained in the silicon dioxide suspension; the furnace having a melting crucible and a gas outlet; Gas is removed from the furnace through the gas outlet; the dew point of the gas exiting the furnace through the gas outlet is less than 0° C.; the first multi-stage filter device has at least first, second and third filter stages, the second filter stage being disposed downstream of the first filter stage and the third filter stage being disposed downstream of the second filter stage; Each filter stage includes at least one filter; the first filter stage has a filter fineness of 5 μm or more, the second filter stage has a filter fineness in the range of 0.5 to 5 μm, and the third filter stage has a filter fineness of 1 μm or less; The filter fineness indicates the smallest particle size that the filter will retain; the first filter stage has a separation rate of 50% or greater, the second filter stage has a separation rate of 95% or greater, and the third filter stage has a separation rate of 99.5% or greater, in each case determined according to ISO 16889.
2. 2. The method of claim 1, wherein the granulation is selected from the group consisting of rotary granulation, spray granulation, centrifugal atomization, freeze granulation and fluidized bed granulation.
3. 3. The method of claim 1 or 2, wherein the silicon component other than silicon dioxide is silicon.
4. 4. The method of claim 3, wherein the one or more silicon components other than silicon dioxide are in an amount of from 10 to 100,000 ppm total, in ppm based on the total weight of silicon dioxide.
5. 3. The method of claim 1 or 2, wherein the dew point of the gas before entering the furnace through the gas inlet is at least 30° C. lower than the dew point of the gas as it exits the furnace through the gas outlet.
6. 3. The method of claim 1 or 2, wherein the furnace is at least partially formed from a material comprising one or more metals selected from molybdenum, tungsten, rhenium, iridium, osmium.
7. The first multi-stage filter device has at least one of the following characteristics: (a) the first filter stage has a filter fineness in the range of 5 to 15 μm; (b) the first filter stage has a separation ratio in the range of 50 to 90%; (c) the second filter stage has a filter fineness in the range of 0.5 to 2 μm; (d) the second filter stage has a separation efficiency of 95% or greater; (e) the third filter stage having a filter fineness of 1.0 μm or less; (f) the third filter stage has a separation efficiency of 99.5% or greater; or a combination of at least two of the methods (a) to (f).
3. The method according to claim 1 or 2, characterized in that
8. 3. The method of claim 1, wherein at least one filter of the first filter device in one of the filter stages selected from the first filter stage, the second filter stage and the third filter stage is designed as a depth filter.
9. 3. The method of claim 1 or 2, wherein the slurry is treated with ultrasound for at least 10 seconds.
10. 3. The method according to claim 1 or 2, wherein the treatment of the slurry with ultrasound is characterized by a power density of up to 600 W / l.
11. 3. The method of claim 1 or 2, wherein the slurry has less than 5% by weight, based on the total weight of the slurry, of an additive to stabilize the slurry.
12. The quartz glass body, At least one of the following characteristics: A] a chlorine content of less than 60 ppm; B] an aluminum content of less than 200 ppb; C] 5 x 10 19 / cm 3 less than 0.05 ODC component; D] content of atoms other than Si, O, H, C of less than 5 ppm; E] log 10 (η(1250℃) / dPas)=11.4~log 10 (η(1250 ° C) / dPas) = 12.9; F] 10 -4 Refractive index homogeneity of less than G] cylindrical; H] tungsten content less than 100 ppb; I] Molybdenum content of less than 100 ppb having 3. The method according to claim 1 or 2, wherein the ppb and ppm are in each case based on the total weight of the quartz glass body.
Citation Information
Patent Citations
Production of quartz glass
JP1992219333A
Production of quartz glass
JP1993024853A
Homogeneous quartz glass fiber and matrix
JP2019502633A
Increasing the silicon content during silica glass preparation
JP2019502641A
Preparation and post-treatment of quartz glass bodies
JP2019504810A