Martensitic stainless steel alloy
A specially formulated martensitic stainless steel alloy with copper additions addresses the mechanical strength loss at high temperatures, ensuring improved tensile strength, hardness, and temperature stability for high-temperature applications.
Patent Information
- Application Number
- JP2021571522
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-09-16
- Filing Date
- 2020-06-04
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2040-06-04
AI Technical Summary
Martensitic stainless steels lose mechanical strength at high temperatures due to their composition and manufacturing process, making them unsuitable for demanding and high-temperature applications, thus reducing their service life.
A martensitic stainless steel alloy with specific compositions (C >0.50~0.60, Si 0.10~0.60, Cu >0.4~1.50, Mn 0.40~0.80, Cr 13.50~14.50, Ni 0~1.20, Mo 0.80~2.50, N 0.050~0.12, V max 0.10, S max 0.03, P max 0.03, Fe and unavoidable impurities) that include intentional additions of copper, resulting in improved tensile strength, hardness, and high ductility, along with enhanced temperature stability.
The alloy maintains high mechanical properties and temperature stability, enabling its use in high-temperature applications with improved fatigue resistance, wear resistance, and increased hardness.
Smart Images

Figure 0007592032000008 
Figure 0007592032000009 
Figure 0007592032000010
Abstract
Description
[Technical field]
[0001] The present disclosure relates to martensitic stainless steel alloys, stainless steel strips including martensitic stainless steel alloys and different components made therefrom. [Background technology]
[0002] Today's martensitic stainless steels generally have high performance and good properties, such as high strength and high ductility, making them suitable for use in a variety of strip applications.
[0003] European Patent EP 303 1942 discloses a martensitic stainless steel that can be used for flapper valves. However, this steel is not suitable for use in demanding and high temperature applications, since due to its composition and the manufacturing process used, it will lose its mechanical strength. Therefore, when used, this steel will not have the necessary mechanical properties and will have a shorter service life.
[0004] Thus, there is a need for martensitic stainless steel alloys that have a combination of good mechanical properties and temperature stability, i.e., that have and maintain good mechanical properties in demanding applications and at high temperatures (temperatures around 300° C.).
[0005] One aspect of the present disclosure is therefore to provide a solution to or reduce this problem. Summary of the Invention
[0006] The present disclosure thus relates to a martensitic stainless steel alloy having the following composition in weight percent (wt.%): C >0.50~0.60; Si 0.10~0.60; Cu >0.4~1.50; Mn 0.40-0.80; Cr 13.50-14.50; Ni 0~1.20; Mo 0.80~2.50; N 0.050~0.12; V max 0.10; S max 0.03; P max 0.03; and the balance being Fe and unavoidable impurities.
[0007] The present disclosure also relates to components comprising or consisting of a martensitic stainless steel alloy. Additionally, the present disclosure also provides methods for manufacturing such components.
[0008] The present invention is based on the discovery that components comprising martensitic stainless steel alloys with a carbon content of more than 0.50 (>0.50) to 0.60 wt.% exhibit improved tensile strength and hardness combined with high ductility, thereby improving fatigue resistance. Furthermore, it has been found that the martensitic stainless steel alloy compositions defined above or below provide good temperature stability, making the material excellent for high temperature applications. This discovery is highly surprising, since typically this high carbon content (>0.50 wt.%) results in a carbide distribution of both primary carbides and coarse carbide particles, which adversely affects the mechanical properties.
[0009] Moreover, in the martensitic stainless steel alloys of the present invention as defined above or below, the intentional addition of copper has been found to improve mechanical properties such as strength. Moreover, it has been surprisingly found that the addition of copper leads to a reduction in the A1 temperature, which has a positive effect on heat treatments, since it allows for a reduction in the temperatures used during austenitization during annealing and hardening, which in turn is beneficial in terms of energy efficiency and costs.
[0010] Furthermore, it has been found that the combination of intentionally added Cu and a large amount of carbon results in high mechanical strength after heat treatment. Without wishing to be bound by any theory, this is believed to be due to the effect of C increasing the strength of martensite, and Cu providing a solid solution strengthening effect on austenite and martensite, as well as a hardening effect due to the formation of clusters and precipitates. The final product thus obtained has improved temperature stability, as the higher mechanical strength allows for higher tempering temperatures after cooling.
[0011] Moreover, articles, such as machine components or strips, comprising or consisting of the martensitic stainless steel alloys defined above or below have a combination of improved fatigue and tensile strength in high temperature environments (temperatures around 300° C.), high hardness and good temperature stability as well as improved wear resistance. [Brief description of the drawings]
[0012] [Figure 1] 1 is a diagram showing the results of a fatigue test, where the relationship R represents the ratio of the fatigue limit to the tensile strength. [Diagram 2] FIG. 1 is a diagram showing the results of evaluation of the thermal stability of alloys. [Diagram 3] 1 is a SEM image of an investigation of Cu particles in an alloy. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The present disclosure provides, in weight percent (wt.%): C >0.50~0.60; Si 0.10~0.60, Mn 0.40-0.80; Cr 13.50-14.50; Ni 0~~1.20; Mo 0.80~2.50; N 0.050~0.12; Cu >0.4~1.50; V max 0.10; S max 0.03; P max 0.03; and the balance being Fe and unavoidable impurities.
[0014] The martensitic stainless steel alloy of the present invention, hereinafter also referred to as "stainless steel alloy" or "stainless steel", has, after hardening and tempering, a microstructure comprising martensite, retained austenite, carbides and carbonitrides, and copper precipitates. The microstructure of the hardened and tempered martensitic stainless steel alloy as defined above or below comprises metal carbonitrides; 23 It is further characterized by the presence of C6 and M7C3 carbides; and / or other types of carbides, where M represents one or more metal atoms.
[0015] The stainless steel alloy of the present invention provides increased hardness without sacrificing temperature stability compared to conventional martensitic stainless steels. High temperature stability is important because it means that the stainless steel alloy can be used in high temperature applications (around 300°C).
[0016] Suitable hardening temperatures for the martensitic stainless steel alloy of the present invention lie in the temperature range of 980-1100°C, for example 1020-1060°C. Suitable tempering temperatures may lie in the range of 200-500°C, depending on the application. By carrying out the tempering process at these temperatures, the components comprising or consisting of the stainless steel alloy of the present invention become temperature stable at high temperatures (approximately 300°C). According to one embodiment, the martensitic stainless steel of the present invention may be tempered at a temperature of 400-450°C. The resulting material will have a sufficiently high hardness for use in the desired application.
[0017] Hardening and tempering times may vary depending on the application and size of the product. Hardening and tempering are carried out in a furnace.
[0018] According to one embodiment, the martensitic alloy of the present invention contains up to 0.5 wt.% of unavoidable impurities, preferably up to 0.3 wt.% of unavoidable impurities, which may occur naturally in the raw materials or recycled materials used to manufacture the stainless alloy.
[0019] Examples of unavoidable impurities are elements and compounds that are not intentionally added, but which cannot be completely avoided because they usually occur as impurities. They are therefore present in the alloy in concentrations that have only a very limited effect on the final properties. The unavoidable impurities present in stainless steel alloys may include, for example, one or more of Co, Sn, Ti, Nb, W, Zr, Ta, B, Ce, and O.
[0020] Small amounts of alloying elements may also be added during the manufacturing process, such as the deoxidation step, or to improve other properties. Examples of such alloying elements are, but are not limited to, Al, Mg, and Ca. Depending on which elements are used, one skilled in the art would know how much is needed. However, according to one embodiment, these elements may be added to the stainless alloy at ≦0.02 wt%.
[0021] The alloying elements of the proposed martensitic stainless alloys are discussed below, however, their effects below should not be construed as limiting.
[0022] Carbon (C) C is metal carbonitride; M 23C6 and M7 are important elements for the formation of C3 carbides; and / or other types of carbides, where M represents one or more metal atoms. C is also important for the hardenability of the steel. Too high a C content, however, in conjunction with other alloying elements, can result in large and unwanted primary carbides being formed during the primary manufacturing stage. Furthermore, a high C content can make martensite more brittle, lower the Ms-temperature at which martensite begins to form, and also increase the amount of retained austenite to too high a level. Thus, the maximum C content of the alloy of the present invention is 0.60wt%, such as 0.58wt%, e.g. 0.56wt%.
[0023] The high carbon content of the alloys of the present invention also surprisingly resulted in a high grain density and a high grain area fraction of carbides. Additionally, and surprisingly, the carbides formed were finely dispersed. The smaller size and greater number of carbides present improves the mechanical properties.
[0024] This may have a positive effect on the wear resistance. A high carbon content is therefore >0.50, such as 0.51 wt%, for example 0.52 wt%, for example 0.53 wt%.
[0025] The amount of C is limited to >0.50-0.60 wt%, preferably 0.51-0.56 wt% in the alloy of the present invention.
[0026] Copper (Cu) In the stainless steel alloy of the present invention, Cu is intentionally added. Cu is an austenite stabilizer and has surprisingly been found to contribute to alternative solid solution strengthening of the steel in the present steel, thereby providing new possibilities for superior properties. Cu will also form a type of cluster and / or precipitate that enhances strength.
[0027] The solubility of Cu in the matrix is greater than 0.4 wt% at equilibrium. In this disclosure, the inventors have discovered that it is important to supersaturate Cu to ensure maximum solid solution strengthening of the martensite and retained austenite phases after hardening and tempering, and that supersaturation also enables cluster strengthening and precipitation hardening. Cu will also improve the corrosion resistance of stainless alloys.
[0028] Therefore, the Cu content is greater than 0.4 and up to 1.50 wt%, for example 0.50-1.50 wt% Cu, for example 0.55-1.30 wt%.
[0029] Silicon (Si) Silicon acts as a ferrite stabilizer and deoxidizer. Silicon also increases carbon activity and contributes to strength increase by solid solution strengthening. Too high a content can result in the formation of unwanted inclusions. The amount of silicon is therefore limited to 0.10-0.60wt%, e.g. 0.20-0.55wt%, e.g. 0.30-0.50wt%.
[0030] Manganese (Mn) Mn is an austenite stabilizer and acts as a deoxidizer. Mn increases the solubility of N and improves hot workability. If the content is too high, it can contribute to the formation of MnS inclusions together with S. The amount of Mn is therefore limited to 0.40-0.80wt%, for example 0.50-0.80wt%.
[0031] Chromium (Cr) Cr is essential for the corrosion resistance of steel, which is determined by the amount of Cr in the steel matrix. Cr is also found in carbides (M 23 It forms Cr, M7C3, carbonitrides) and increases the solubility of C and N. Cr is a ferrite stabilizer and too much Cr can lead to the formation of delta ferrite. The amount of Cr is therefore limited to 13.50-14.50 wt%.
[0032] Molybdenum (Mo) Mo is a ferrite stabilizer and a strong carbide former. Mo has a positive effect on both the corrosion resistance and hardenability of the steel. Mo also contributes to improving the ductility. Since Mo is an expensive element, the content should not be higher than necessary for economic reasons. The amount of Mo is therefore limited to 0.80-2.50 wt%, preferably 0.80-2.00 wt%, more preferably 0.90-1.30 wt%.
[0033] Nitrogen (N) N is an austenite stabilizer and increases the strength of steel by interstitial solid solution strengthening. N contributes to increasing the hardness of martensite. N will form nitrides and carbonitrides. Too much N, however, will reduce hot workability. The amount of N is therefore limited to 0.050-0.12wt%, preferably 0.050-0.10wt%, for example 0.055-0.085wt%.
[0034] Nickel (Ni) Ni is an austenite stabilizer and reduces the solubility of C and N. Since Ni is an expensive element, the content should be kept low for economic reasons, and Ni is usually not intentionally added to the stainless steel alloy of the present invention. The amount of Ni should be ≦1.20wt%, preferably ≦0.40wt%, more preferably ≦0.35wt%. According to one embodiment, Ni is 0.15-0.35wt%.
[0035] Vanadium(V) V is a strong carbide former and limits grain growth. As a carbide former, V may be present in martensitic alloys or may be added intentionally. It may also be present due to recycled materials, in which case it is considered an impurity. The content will also depend on the source of chromium. However, too high a V content can reduce ductility and hardenability and lead to unwanted primary carbides. When present in stainless steel alloys, the amount of V is therefore limited to 0.010-0.10 wt%, e.g. 0.030-0.10 wt%.
[0036] Rin(P) P causes embrittlement. P is normally not added and should be limited to ≦0.03 wt%.
[0037] Sulfur (S) S will adversely affect hot workability and, if too much is added, will cause the formation of MnS inclusions. S is normally not added and should be limited to ≦0.03 wt%.
[0038] According to one embodiment, the stainless steel alloy of the present invention comprises any of the above-mentioned alloying elements in any of the ranges given above. According to another embodiment, the stainless steel alloy of the present invention consists of any of the above-mentioned alloying elements in any of the ranges given above.
[0039] Thus, the alloys of the present invention and articles constructed therefrom will have superior strengthening due to maximized solid solution hardening from the intentional addition of Cu in the ranges disclosed herein, and precipitation hardening from finely divided carbides. Additionally, ductility is improved by the composition of the microstructure.
[0040] The martensitic stainless steel alloys may be suitably manufactured in the form of components, for example strip, but may also be manufactured in the form of wires, rods, bars, tubes, and the like.
[0041] The martensitic stainless steel alloys of the present invention can be used as valve components for different machine components, such as compressors, e.g., flapper valves. The martensitic stainless steels of the present invention are also suitable for other applications where high fatigue strength and / or wear resistance and edge performance are desirable.
[0042] According to one embodiment, the stainless steel alloy of the present invention can be produced according to the following: - Melting - the melting process can be carried out using an EAF - Electric Arc Furnace - followed by the AOD process and optional final conditioning; - Casting - casting into the desired shape, e.g. blooms of 100-600 mm; - Heating - Heat the bloom until the material reaches a temperature of 1200-1350 °C; - Rolling - The bloom is hot rolled into strip. Hot rolling can be performed with multiple passes depending on the roll mill being used. This step can optionally include one or more heat treatment steps if found necessary to obtain the desired strip dimensions. - Winding - winding of strip, winding temperature after cooling is about 500~800℃ - Annealing - annealing of hot-rolled strip at 700-900 ° C for at least 1 h. - Optional surface treatment - Rolling - e.g. cold rolling to a final thickness of 0.040-3mm. - Optional annealing - An intermediate annealing at a temperature of about 650-800°C may be necessary for recrystallization. - Hardening - Hardening can be carried out in a continuous hardening line, including the following steps: austenitizing, quenching, additional cooling, tempering, cooling to room temperature and polishing. The speed of the hardening line depends on the material thickness or mass flow rate and the size of the furnace(s) and can be 100-1000 m / h. The length of the austenitizing and tempering furnaces is approximately the same. The austenitizing temperature is 950-1100°C. Quenching should be done so that the material temperature falls rapidly, usually within 2 minutes, to below about 500°C to avoid brittleness or loss of corrosion resistance. Additional cooling is optionally performed to pass the material below the Ms temperature to obtain the desired level of retained austenite. Cooling temperatures are usually applied at room temperature, but can range from -100 to 100°C depending on the end use. Tempering can be set at 250 to 500°C depending on the desired ultimate tensile strength.
[0043] The present disclosure is further illustrated by the following non-limiting examples. EXAMPLES
[0044] Example 1 Several alloys were produced by melting using a vacuum induction melting furnace (VIM). The elemental composition of the alloys in wt% is shown in Table I. The balance is Fe and unavoidable impurities. If no value is given for a particular element, the amount of that element is below the detection limit. Alloys 1, 2 and 3 are included as comparative examples, while the remaining alloys represent various embodiments of stainless alloys according to the present disclosure. The alloys were produced as described below and were stainless alloys. TIFF0007592032000001.tif78170
[0045] From the heats, samples in the form of cylindrical test rods were prepared for testing.
[0046] The process flow is therefore; The raw materials are melted in a vacuum induction melting furnace (VIM), casting, Before hot working, preheat to 700℃ (30 min), followed by heat treatment at 1150℃ (30 min), Annealing (825-875℃ for 6h) and Machining of specimens; followed by hardening and tempering It was.
[0047] The test samples were hardened at 1030°C and 1050°C, followed by quenching (to RT) and then tempering at 450°C (for hardening at 1050°C) and 250 and 450°C (for hardening at 1030°C) for 2h, the results of which can be seen in Tables IIA and IIB.
[0048] These hardness (HV1) measurements were carried out according to SS-EN ISO 6507. The values are the average of 5 measurements. TIFF0007592032000002.tif87170
[0049] As can be seen in Table IIA, the results showed an increase in hardness for the two sets of data hardened at 1030°C. The data showed a clear increase in hardness even at the higher tempering temperatures, indicating an increase in hardness with the addition of Cu.
[0050] Table IIA further shows that tempering at a higher temperature, 450°C, resulted in higher hardness (and therefore higher tensile strength) of the alloy of the present invention, which means that the alloy of the present invention will have better performance when used in high temperature applications. TIFF0007592032000003.tif75170
[0051] Table IIB shows that the hardness of the alloys of the present invention is higher than the comparative alloys at 1050 HV, 450° C. This suggests that the alloys of the present invention are suitable for use in high temperature applications as they retain their higher performance.
[0052] Fatigue measurement TIFF0007592032000004.tif24170
[0053] To measure the fatigue properties of the alloy, alloy 11 was manufactured, having the above composition, with a final thickness of 0.305 mm, and then tested for fatigue properties using a variable tensile testing machine AMSLER with a 10% preload operating at a resonance of about 80 Hz, using the step method. * 10 6 Several specimens were manufactured, each consisting of a 10 mm central fuselage and a 15 mm length.
[0054] The method involves exposing a complete cross section to the applied stress conditions, thereby testing the material properties in a larger volume for limiting factors. The specimens are tumbled to ensure proper edge and high surface residual stresses. The fatigue test performed has a 50% chance of failure.
[0055] In Figure 1 the results of the fatigue test are shown. The relationship R represents the ratio of fatigue limit to tensile strength. The obtained standard deviation is shown for each box size, respectively. As can be seen, the material of the invention exhibits a fatigue limit of 1505 MPa, whereas the reference material (based on EN 1.4031) exhibits 1390.
[0056] Precipitate Table III. Compositions of alloys used to measure carbides. Alloy A is within the scope of this disclosure. Alloys A (as-produced HV1 593), B (as-produced HV1 520), C (as-produced HV1 552) and D (as-produced HV1 612) are comparative alloys. TIFF0007592032000005.tif55170TIFF0007592032000006.tif42170
[0057] As can be seen from the tables of the present disclosure, the alloys of the present disclosure have particle densities greater than 50. TIFF0007592032000007.tif26170
[0058] The data in Table V was obtained from image processed SEM images, an example of which is shown in Figure 3. The Cu particles of the alloy of the present invention are stable below the A1 temperature according to Thermo Calc calculations. The presence of Cu particles in the image indicates that in addition to the maximized solid solution, there are also sub-visible Cu clusters and sub-visible finer Cu particles. Both the Cu precipitates and the Cu clusters will contribute to the mechanical properties.
[0059] The thermal stability of some of the alloys in Table III was evaluated, and the results are shown in Figure 2.
[0060] Figure 2 shows that alloy D will lose its properties if exposed to temperatures higher than those at which it is stabilized during tempering. In the case of alloy A, higher hardness and therefore higher tensile strength can be obtained without compromising thermal stability, which is shown as a hardness that is almost unaffected throughout the temperature range.
Claims
1. In weight percent (wt.%): C greater than 0.5 and equal to or less than 0.60; Si 0.10~0.60, Mn 0.40-0.80; Cr 13.50-14.50; Ni 0-1.20; Mo 0.80-2.50; N 0.050-0.12; Cu more than 0.4 and not more than 1.50; V maximum 0.10; S maximum 0.03; P maximum 0.03; and the balance being Fe and unavoidable impurities.
2. 2. The martensitic stainless steel alloy according to claim 1, wherein the Si content is 0.20 to 0.55 wt %.
3. 3. The martensitic stainless steel alloy according to claim 1, wherein the Mn content is 0.50 to 0.80 wt %.
4. The martensitic stainless steel alloy according to any one of claims 1 to 3, wherein the content of Mo is 0.80 to 2.00 wt%.
5. 5. The martensitic stainless steel alloy according to claim 1, wherein the Ni content is 0.80 wt% or less.
6. The martensitic stainless steel alloy according to any one of claims 1 to 5, wherein the N content is 0.050 to 0.10 wt%.
7. 7. The martensitic stainless steel alloy according to claim 1, wherein the V content is 0.030 to 0.10 wt %.
8. The martensitic stainless steel alloy according to any one of claims 1 to 7, wherein the C content is 0.51 to 0.60 wt%.
9. 9. A martensitic stainless steel alloy according to any one of the preceding claims, wherein the stainless steel alloy contains 0.50-1.5 wt% Cu.
10. 10. A stainless steel article comprising the martensitic stainless steel alloy of any one of claims 1 to 9.
11. The stainless steel article of claim 10, wherein the article is a strip.
12. 12. The stainless steel article of claim 10 or 11, wherein the article is cold rolled, hardened and tempered.
13. The microstructure is a metal carbonitride; 23 C 6 and M. 7 C 3 13. The stainless steel article of claim 12, characterized by the presence of carbides, where M represents one or more metal atoms; and / or other types of carbides.
14. 14. The stainless steel article of claim 12 or 13, wherein the microstructure comprises Cu precipitates and / or clusters.
Citation Information
Patent Citations
Martensitic stainless steel wire rod and production method thereof
CN105525226A
High abrasion resisting stainless steel for vehicle brake disc and manufacturing method of high abrasion resisting stainless steel
CN109280862A
Stainless steel strip for flapper valve
JP2017508863A
martensitic stainless steel and method of manufacturing it
KR1020130000841A