Method for inspecting silicon carbide semiconductor device
The integrated inspection method for silicon carbide semiconductor devices reduces costs and complexity by combining on-voltage and body diode energization steps, enhancing screening accuracy through temperature-dependent voltage measurements.
Patent Information
- Application Number
- JP2021000361
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-01-05
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2041-01-05
AI Technical Summary
Conventional methods for inspecting silicon carbide semiconductor devices require multiple steps and different devices for on-voltage and body diode energization measurements, increasing costs and complexity.
A method that integrates on-voltage measurement and body diode energization into a single inspection process, using a silicon carbide semiconductor device with specific regions and electrodes, and applying pulse signals to measure voltage differences before, during, and after diode energization, allowing simultaneous determination of device quality.
Reduces the number of inspection steps, improves screening accuracy by measuring voltage fluctuations at different temperatures, and enables efficient identification of non-defective semiconductor chips.
Smart Images

Figure 0007593114000001 
Figure 0007593114000002 
Figure 0007593114000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for inspecting a silicon carbide semiconductor device. [Background technology]
[0002] Conventionally, in a MOS-type silicon carbide (SiC) semiconductor device having a MOS gate (an insulated gate having a three-layer structure of metal-oxide-semiconductor), it is known that stacking faults grow when a current flows through a parasitic pn diode (body diode (BD)) formed at the pn junction between a p-type base region and an n-type drift region, and the resistance becomes high in the area where the stacking fault grows, making it difficult for current to flow and increasing the on-voltage Von.
[0003] For example, in a semiconductor circuit device constructed by combining multiple MOS-type silicon carbide semiconductor devices (semiconductor chips), a semiconductor chip in which stacking faults have grown makes it difficult for current to flow, and the amount of current flowing into other semiconductor chips connected in parallel to the semiconductor chip becomes relatively large to the extent that the current flow into the semiconductor chip becomes difficult. As a result, the current load of each semiconductor chip may vary from the design conditions, and the reliability of the semiconductor circuit device may decrease.
[0004] In order to prevent adverse effects on semiconductor circuit devices due to fluctuations in the on-voltage Von of MOS type silicon carbide semiconductor devices (semiconductor chips) caused by such stacking faults, an inspection method is known in which a current is passed through the body diode before the shipment of the semiconductor chip, the on-voltage Von of the MOS type semiconductor device or the forward voltage Vf of the body diode is measured before and after the body diode is passed through, and semiconductor chips with large fluctuations are screened (selected).
[0005] A conventional method for inspecting silicon carbide semiconductor devices has been proposed in which a pulse current is passed through a body diode (the body diode is energized) to accelerate degradation of a MOS type silicon carbide semiconductor device to grow stacking faults, the on-resistance of the body diode is measured before and after the pulse current is passed, and the pass / fail status of the MOS type silicon carbide semiconductor device is judged based on the rate of increase in the on-resistance of the body diode before and after the pulse current is passed (see, for example, Patent Document 1).
[0006] Furthermore, as another conventional method for inspecting silicon carbide semiconductor devices, a method has been proposed in which a forward current is passed through a body diode (the body diode is energized) to grow stacking faults, the on-voltage of the MOS silicon carbide semiconductor device is measured before and after the body diode is energized, and MOS silicon carbide semiconductor devices in which the rate of change in the on-voltage measured before and after the body diode is energized is lower than 3% are selected as non-defective products (see, for example, Patent Document 2). [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2015-065250 A [Patent Document 2] JP 2020-150181 A Summary of the Invention [Problem to be solved by the invention]
[0008] However, in the above-mentioned Patent Documents 1 and 2, in order to check the characteristic fluctuation of a MOS-type silicon carbide semiconductor device (semiconductor chip) before and after the body diode is energized, it is necessary to perform an on-voltage measurement (or on-resistance measurement), body diode energization, and on-voltage measurement (or on-resistance measurement) in that order. Since the on-voltage measurement and body diode energization are performed using different inspection devices, the number of steps in the screening inspection increases, which is a factor in increasing costs. For this reason, it is desired to establish a method for screening inspection of a semiconductor chip in which the on-voltage fluctuates when the body diode is energized, with as few steps as possible.
[0009] In order to solve the above-mentioned problems associated with the conventional techniques, an object of the present invention is to provide a method for inspecting a silicon carbide semiconductor device that can reduce the number of steps in a screening inspection of a semiconductor chip. [Means for solving the problem]
[0010] In order to solve the above-mentioned problems and achieve the object of the present invention, a method for inspecting a silicon carbide semiconductor device according to the present invention is a method for inspecting a silicon carbide semiconductor device including a semiconductor chip made of silicon carbide, a first semiconductor region of a first conductivity type, a second semiconductor region of a second conductivity type, a third semiconductor region of the first conductivity type, a gate insulating film, a gate electrode, a first electrode, and a second electrode, and has the following features. The first semiconductor region is provided inside the semiconductor chip. The second semiconductor region is provided between a front surface of the semiconductor chip and the first semiconductor region. The third semiconductor region is selectively provided between the front surface of the semiconductor chip and the second semiconductor region. The gate insulating film is provided in contact with a region of the second semiconductor region between the third semiconductor region and the first semiconductor region. The gate electrode is provided on the opposite side of the second semiconductor region with the gate insulating film interposed therebetween. The first electrode is electrically connected to the second semiconductor region and the third semiconductor region.
[0011] The second electrode is provided on the back surface of the semiconductor chip. A first step is performed in which a parasitic diode formed by a pn junction between the second semiconductor region and the first semiconductor region is energized by inputting a first pulse signal having a predetermined period. A second step is performed in which a predetermined first current is caused to flow from the second electrode to the first electrode in the semiconductor chip by inputting an on-signal of a predetermined second pulse signal, and a positive first voltage applied to the second electrode with respect to the first electrode is measured. A third step is performed in which the input of the first pulse signal is terminated to terminate the energization of the parasitic diode. After the first step and before the third step, a fourth step is performed in which a first difference between two first voltages obtained by performing the second step at different timings on the semiconductor chip heated by the first step is calculated. A fifth step is performed in which the semiconductor chip having the first difference within a first predetermined range is selected as a non-defective product.
[0012] In addition, the method for inspecting a silicon carbide semiconductor device according to the present invention, in the above-mentioned invention, further includes a sixth step of calculating a second difference between the first voltage obtained by performing the second step on the semiconductor chip before the first step and the first voltage obtained by performing the second step on the semiconductor chip whose temperature has been lowered after the third step. In the sixth step, the semiconductor chip for which the first difference is within the first predetermined range and the second difference is within a second predetermined range is selected as a non-defective product.
[0013] Furthermore, in the method of inspecting a silicon carbide semiconductor device according to the present invention, in the above-mentioned invention, the fourth step calculates the first difference between the first voltage obtained by performing the second step at an early stage of current flow through the parasitic diode and the first voltage obtained by performing the second step after a predetermined time of current flow through the parasitic diode has elapsed.
[0014] Furthermore, in the above-described invention, a method for inspecting a silicon carbide semiconductor device according to the present invention includes a seventh step of flowing a second current in a forward direction through the parasitic diode by inputting an on-signal of a predetermined third pulse signal, and measuring a second positive voltage applied to the first electrode relative to the second electrode, and an eighth step of calculating a temperature of the semiconductor chip based on the second voltage. The method is characterized in that the temperature of the semiconductor chip is acquired by the seventh step and the eighth step, and the second step is performed after confirming that the temperature of the semiconductor chip is a predetermined set temperature.
[0015] In addition, in the method of inspecting a silicon carbide semiconductor device according to the present invention, in the above-mentioned invention, the seventh step measures the second voltage when the second current, 1 / 1000 of a rated current of the parasitic diode, flows through the parasitic diode. The eighth step calculates a temperature of the semiconductor chip based on the second voltage obtained by performing the seventh step before the first step and the second voltage obtained by performing the seventh step after the first step.
[0016] Furthermore, in the method of inspecting a silicon carbide semiconductor device according to the present invention, in the above-mentioned invention, in the seventh step, an on signal of the third pulse signal is input at a timing different from the timing of input of the on signals of the first pulse signal and the second pulse signal.
[0017] In addition, in the method for inspecting a silicon carbide semiconductor device according to the present invention, in the above-mentioned invention, in the second step, an on signal of the second pulse signal is input at a timing different from that of the on signal input of the first pulse signal.
[0018] According to the above-described invention, the first voltage, which is a judgment factor for screening, is measured while the body diode is conducting, and the judgment factor for screening can be obtained almost simultaneously with the end of the conduction of the body diode. Effect of the Invention
[0019] Advantageous Effects of Invention According to the method for inspecting a silicon carbide semiconductor device according to the present invention, it is possible to reduce the number of steps for screening a semiconductor chip. [Brief description of the drawings]
[0020] [Figure 1] 1 is a cross-sectional view showing a state in which the silicon carbide semiconductor device according to the embodiment is operating; [Diagram 2] 2 is a flowchart illustrating a method for inspecting a silicon carbide semiconductor device according to an embodiment. [Diagram 3] 3 is a waveform diagram showing a current waveform applied to the silicon carbide semiconductor device according to the embodiment during the inspection of FIG. 2. [Figure 4] FIG. 13 is a characteristic diagram showing the measurement variation of the drain-source voltage of a MOSFET at room temperature in an experimental example. [Diagram 5] FIG. 13 is a characteristic diagram showing the measurement variation of the drain-source voltage of a MOSFET at high temperature (set temperature T1=175° C.) in an experimental example. [Figure 6] FIG. 13 is a characteristic diagram showing measurement variations in forward voltage of a body diode of a comparative example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] A preferred embodiment of the method for inspecting a silicon carbide semiconductor device according to the present invention will be described in detail below with reference to the accompanying drawings. In this specification and the accompanying drawings, in a layer or region prefixed with n or p, electrons or holes are the majority carriers, respectively. In addition, + and - attached to n or p respectively mean that the impurity concentration is higher and lower than that of a layer or region not prefixed with that. In the following description of the embodiment and the accompanying drawings, the same reference numerals are attached to similar configurations, and duplicated explanations will be omitted.
[0022] (Embodiment) The method for inspecting a silicon carbide semiconductor device according to the embodiment will be described taking a MOSFET (Metal Oxide Semiconductor Field Effect Transistor: a MOS type field effect transistor having an insulated gate with a three-layer structure of metal (gate electrode)-oxide film (gate insulating film)-semiconductor) as an example, but is similarly applicable to other MOS type silicon carbide semiconductor devices having a MOS gate. FIG. 1 is a cross-sectional view showing a state during operation of a silicon carbide semiconductor device according to the embodiment. (a) and (b) of FIG. 1 respectively show a MOSFET when it is on and a body diode (BD) when it is conducting.
[0023] First, the structure of a silicon carbide semiconductor device according to an embodiment will be described. A silicon carbide semiconductor device 10 according to an embodiment shown in Fig. 1 is a vertical MOSFET having a MOS gate on the front surface side of a semiconductor substrate (semiconductor chip) 30 made of silicon carbide (SiC). + On the front surface of the starting substrate 31, n-type buffer regions 2a, - The epitaxial layers 32 to 34 that become the n-type drift region 2b and the p-type base region 4 are epitaxially grown in sequence. The main surface of the semiconductor substrate 30 facing the p-type epitaxial layer 34 is the front surface, and the n-type + The main surface on the mold starting substrate 31 side is referred to as the back surface.
[0024] n + The starting substrate 31 is n + The n-type drain region 1 is an n-type buffer region 2a. + Alternatively, the n-type buffer region 2a may have a two-layer structure in which a low-concentration n-type epitaxial layer and a high-concentration n-type epitaxial layer having a higher impurity concentration than the low-concentration n-type epitaxial layer are stacked in this order on the starting substrate 31. - Holes (positive holes) generated at the pn junction interface with the n-type drift region 2b recombine in the n-type buffer region 2a to form n + The n-type buffer region 2a functions to prevent the n-type starting substrate 31 from being reached. +This makes it possible to suppress the growth of stacking faults in epitaxial layers 32 to 34 from mold starting substrate 31.
[0025] The n-type buffer region 2a may not be provided. When the n-type buffer region 2a is not provided, + On the front surface of the starting substrate 31, - n-type drift region 2b - A type epitaxial layer 33 is epitaxially grown. - The n-type drift region 2b is - The n-type epitaxial layer 33 includes an n-type current diffusion region 3 and first and second p-type epitaxial layers 32, which will be described later. + Type regions 21, 22 and n + This is the part excluding the mold region 23. - The n-type drift region 2b is connected to the n-type current diffusion region 3 and the first and second p-type + Type regions 21, 22 and n + The dopant is provided between the n-type region 23 and the n-type buffer region 2a so as to be in contact with these regions.
[0026] The p-type base region 4 is a region of the p-type epitaxial layer 34, which will be described later. ++ The source region 5 and the p ++ The p-type base region 4 is a portion excluding the n-type contact region 6. - The n-type drift region 2b is provided between the n-type drift region 2b. - An n-type current diffusion region 3, which is a so-called current spreading layer (CSL) that reduces the spreading resistance of carriers, may be provided between the p-type drift region 2b and the p-type base region 4 in contact with these regions. The n-type current diffusion region 3 is located closer to the n-type drift region 2b than the bottom surface of a trench 7 described later. + The trench reaches a deep position on the drain region 1 side.
[0027] The MOS gate is a p-type base region 4, ++ Type source region 5, p ++ The trench gate structure is composed of a contact region 6, a trench 7, a gate insulating film 8, and a gate electrode 9, and is arranged for each unit cell (functional unit of the element) of the MOSFET.++ Type source region 5 and p ++ The contact regions 6 are selectively provided between the front surface of the semiconductor substrate 30 and the p-type base region 4, in contact with the p-type base region 4, and exposed on the front surface of the semiconductor substrate 30. Exposure on the front surface of the semiconductor substrate 30 means that the contact regions 6 are in contact with a source electrode 13 (described later) through a contact hole in an interlayer insulating film 11 (described later).
[0028] p ++ The p-type contact region 6 may not be provided. ++ Instead of the p-type contact region 6, the p-type base region 4 is exposed on the front surface of the semiconductor substrate 30. + Type regions 21, 22 and n + The n-type region 23 is located closer to the bottom of the trench 7 than the n-type region 23. + The first and second p-type drain regions are disposed at a deep position on the side of the first and second p-type drain regions. + The mold regions 21 and 22 have the function of reducing the electric field applied to the bottom surface of the trench 7. + The first p-type region 21 is provided apart from the p-type base region 4 and faces the bottom surface of the trench 7 in the depth direction. + The mold region 21 may be electrically connected to the source electrode 13 at a portion not shown.
[0029] 1st p. + The mold region 21 may surround the bottom surface of the trench 7 and be exposed to the bottom surface of the trench 7. The exposure to the bottom surface of the trench 7 means that the bottom surface of the trench 7 is in contact with the gate insulating film 8. + The mold region 22 is formed between the adjacent trenches 7 and has a first p + The n-type region 21 and the trench 7 are spaced apart from each other, and are in contact with the p-type base region 4. + The mold region 23 is a second p + Type region 22 and n - The n-type drift region 2b is provided between the n-type drift region 2b and in contact with these regions. + The first p of the bottom surface of the trench 7 is formed by the mold region 23. + The breakdown voltage ensured by the mold region 21 is the second p between the adjacent trenches 7. +This is higher than the withstand voltage ensured by the mold region 22 .
[0030] Trench 7 is n ++ The n-type current diffusion region 3 (or the n-type current diffusion region 3 if the n-type current diffusion region 3 is not provided) penetrates the p-type source region 5 and the p-type base region 4. - The trench 7 extends from the source pad 14 to the gate electrode 9 (which is a first region of the trench 7 that extends from the source pad 14 to the gate electrode 9). A gate electrode 9 is provided inside the trench 7 with a gate insulating film 8 interposed therebetween. The gate electrodes 9 of all the unit cells are electrically connected to a gate pad (electrode pad: not shown). An interlayer insulating film 11 covers the gate electrode 9. A barrier metal 12 may be provided on the entire surface between the interlayer insulating film 11 and a source pad 14 (described later) to prevent diffusion of metal atoms from the source pad 14 side to the gate electrode 9 side, for example.
[0031] The source electrode 13 is an n-type semiconductor layer exposed through a contact hole in the interlayer insulating film 11. ++ Type source region 5 and p ++ Type contact region 6(p ++ When the n-type contact region 6 is not provided, the n-type contact region 6 is in contact with the p-type base region 4). ++ Type source region 5 and p ++ The source pad (electrode pad) 14 is provided on substantially the entire front surface of the semiconductor substrate 30 so as to fill the contact hole of the interlayer insulating film 11. The drain electrode 15 is provided on the rear surface (n + The back surface of the starting substrate 31 is provided on the entire surface of the substrate. + Type drain region 1(n + The mold is electrically connected to a starting substrate 31).
[0032] The operation of the silicon carbide semiconductor device 10 according to the embodiment will now be described. When a gate voltage equal to or greater than a gate threshold voltage is applied to the gate electrode 9 while a positive voltage (drain-source voltage Vds) with respect to the source pad 14 is applied to the drain electrode 15, a channel (n-type inversion layer) is formed in the portion of the p-type base region 4 along the trench 7. + From the n-type drain region 1 to the n-type buffer region 2a, -Through the drift region 2b and the channel ++ A drain-source current Ids flows toward the type-source region 5, and the MOSFET (silicon carbide semiconductor device 10) turns on (FIG. 1(a)).
[0033] On the other hand, when a gate voltage less than the gate threshold voltage is applied to the gate electrode 9 while a positive voltage with respect to the source pad 14 is applied to the drain electrode 15, the first and second p + The p-type regions 21 and 22 and the p-type base region 4, and the n-type current diffusion regions 3 and + type area 23, n - The pn junction between the n-type drift region 2b and the n-type buffer region 2a is reverse biased, so that the drain-source current Ids does not flow and the MOSFET remains in the off state. A depletion layer spreads from the pn junction, and the electric field applied to the gate insulating film 8 on the bottom surface of the trench 7 located on the source electrode 13 side of the pn junction is relaxed.
[0034] When the MOSFET is turned off, a negative voltage (forward voltage Vf of the body diode) is applied to the drain electrode 15 with respect to the source pad 14. + The p-type regions 21 and 22 and the p-type base region 4, and the n-type current diffusion regions 3 and + type area 23, n - A forward current If flows through a parasitic pn diode (body diode: BD) formed by a pn junction between the n-type drift region 2b and the n-type buffer region 2a (FIG. 1(b)). As described above, when a forward current If flows through the body diode of the MOSFET (when BD is energized), stacking faults grow inside the semiconductor substrate 30, and the on-voltage Von of the MOSFET increases.
[0035] Therefore, to prevent the on-voltage Von of the MOSFET from fluctuating due to the conduction of the body diode when the silicon carbide semiconductor device 10 (semiconductor chip: product) according to the embodiment is used, a screening test is performed before the product is shipped to screen (select) semiconductor chips whose on-voltage Von of the MOSFET does not fluctuate by conducting the body diode in advance. The on-voltage Von of the MOSFET is the lower limit drain-source voltage Vds required to turn on the MOSFET. Next, a method of testing (screening test method) for the silicon carbide semiconductor device 10 according to the embodiment will be described.
[0036] Fig. 2 is a flow chart showing a method for inspecting a silicon carbide semiconductor device according to an embodiment. Fig. 3 is a waveform diagram showing a current waveform flowing through the silicon carbide semiconductor device according to the embodiment during the inspection of Fig. 2. As shown in Fig. 2, in the method for inspecting a silicon carbide semiconductor device according to the embodiment, first, a semiconductor substrate (semiconductor chip) 30 on which the silicon carbide semiconductor device 10 according to the embodiment has been fabricated (manufactured) is placed on a conductive stage (not shown) of an inspection device with the back surface facing the stage. As a result, a drain electrode 15 on the back surface of the semiconductor substrate 30 is connected to a measurement device (tester: not shown).
[0037] Next, a plurality of different probes (not shown) are pressed against the source pad 14 and gate pad (not shown) of the semiconductor substrate 30 on the stage (or the electrode pads are pressed against the probes), and these electrode pads are electrically connected to a measuring device via the probes (step S1). The plurality of probes and the stage form a set of input / output terminals. The plurality of probes connected to the source pad 14 and gate pad, respectively, may include a sense probe connected to the electrode pad of a sense element (not shown) for protecting and controlling the MOSFET (see FIG. 1), which is the main element.
[0038] Next, input of a temperature measurement pulse signal (FIG. 3(c)) is started (step S2). The temperature measurement pulse signal may be either a single pulse or a continuous pulse, as long as it is turned on (on signal input) at the timing when a BD energization pulse signal (FIG. 3(a)) described later is turned off (off signal input) and at the timing when a Von measurement pulse signal (FIG. 3(d)) described later is turned off. When the temperature measurement pulse signal is a single pulse, an on signal for one period of the temperature measurement pulse signal is input at a predetermined timing. When the temperature measurement pulse signal is a continuous pulse, the temperature measurement pulse signal is turned on and off continuously in a predetermined period.
[0039] When a current sense of the main element is provided on the semiconductor substrate 30, a temperature measurement pulse signal may be input to the current sense via the sense probe, and the temperature Tm of the semiconductor substrate 30 may be calculated as described below using the forward voltage Vf of the body diode of the current sense. In this case, a BD energization pulse signal and a Von measurement pulse signal are input to the main element via the remaining probes excluding the sense probe. For this reason, the on-timing of the temperature measurement pulse signal may overlap with the on-timing of the BD energization pulse signal and the on-timing of the Von measurement pulse signal, improving the degree of freedom in design.
[0040] Furthermore, when a temperature sensor for the main element is provided on the semiconductor substrate 30, the temperature Tm of the semiconductor substrate 30 may be measured using the temperature sensor instead of the method for calculating the temperature Tm of the semiconductor substrate 30 described later. The current sensor is a MOSFET having the same structure as the main element. The current sensor is connected in parallel to the main element, operates under the same conditions as the main element, and has the function of detecting an overcurrent (OC) flowing through the main element. The temperature sensor is a diode, and has the function of detecting the temperature of the MOSFET serving as the main element by utilizing the temperature characteristics of the diode.
[0041] The temperature measurement pulse signal is a signal for calculating the temperature Tm of the semiconductor substrate 30. With the MOSFET in an off state, an on signal of the temperature measurement pulse signal is input between the source pad 14 and the drain electrode 15 via the probe, and a forward current If flows through the body diode for the duration of the on signal of the temperature measurement pulse signal (on pulse width). The forward voltage Vf of the body diode at this time is obtained as the voltage Vm1 applied to the semiconductor substrate 30 when the on signal of the temperature measurement pulse signal is input. The temperature Tm of the semiconductor substrate 30 is calculated using the following formula (1) utilizing the temperature characteristics of the diode (when the temperature rises, the forward voltage Vf falls).
[0042] Tm = T0 + (Vm0 - Vm1) × α (1)
[0043] In the above formula (1), Tm is the temperature of the semiconductor substrate 30. T0 is the stage temperature before the body diode is energized. Vm0 and Vm1 are voltages applied to the semiconductor substrate 30 by inputting an ON signal of a temperature measurement pulse signal before and during the energization of the body diode, respectively. α is the temperature coefficient of the body diode, and is obtained in advance before the screening test. The temperature Tm of the semiconductor substrate 30 needs to be calculated at least once each before the body diode is energized (at room temperature (RT)), at the beginning of the energization (at high temperature), immediately before the end of the energization (at high temperature), and after the energization (at room temperature), and does not need to be checked constantly.
[0044] Specifically, the temperature Tm of the semiconductor substrate 30 may be calculated at least once each near the processing (Von measurement) of steps S3, S5, S6, and S9 described below (for example, at the timings just before Von measurement shown as Tm0, Tm1, and Tm2 in FIG. 3(c)). This makes it possible to obtain the transition of the temperature Tm of the semiconductor substrate 30 from the processing of step S2 to the processing of step S12 described below (FIG. 3(b)). FIG. 3(c) shows a state in which a temperature measurement pulse signal is input at a predetermined period (continuous pulse). In this case, the temperature Tm of the semiconductor substrate 30 may be calculated each time the temperature measurement pulse signal is turned on.
[0045] When the on signal of the temperature measurement pulse signal is input only when the temperature Tm of the semiconductor substrate 30 is calculated (the temperature measurement pulse signal is a single pulse), for example, instead of the processing of step S2 (start of input of the temperature measurement pulse signal) and the processing of step S12 (end of input of the temperature measurement pulse signal), the on signal of the temperature measurement pulse signal may be input and the temperature Tm of the semiconductor substrate 30 may be calculated between the processing of step S1 and the processing of step S3, between the processing of step S4 and the processing of step S5, between the processing of step S5 and the processing of step S6, and between the processing of step S8 and the processing of step S9.
[0046] In order to turn off the MOSFET when an ON signal of the temperature measurement pulse signal is input, a gate voltage Vg less than the gate threshold voltage may be applied to the gate pad. Preferably, a negative gate voltage Vg (e.g., Vg=-10V) is applied to the gate pad to completely turn off the MOSFET. The strength (amplitude) of the temperature measurement pulse signal is set to a level that does not cause the temperature Tm of the semiconductor substrate 30 to rise due to the ON signal input of the temperature measurement pulse signal. Specifically, the strength of the temperature measurement pulse signal is, for example, a strength that causes a forward current If of about 1 / 1000 of the rated current to flow through the body diode due to the ON signal input of the temperature measurement pulse signal.
[0047] Hereinafter, an example will be described in which the temperature Tm of the semiconductor substrate 30 is calculated immediately before measuring Von. First, a stage temperature T0 is acquired as the temperature Tm0 of the semiconductor substrate 30 before the body diode is energized. This stage temperature T0 corresponds to room temperature (for example, about 25°C). In addition, as described above, with the MOSFET turned off, an on-signal of a temperature measurement pulse signal with a predetermined strength is input to pass a predetermined forward current If (set current) through the body diode, and the forward voltage Vf of the body diode at this time is measured, and this forward voltage Vf is acquired as the voltage Vm0 applied to the semiconductor substrate 30 before the body diode is energized.
[0048] Next, the on-voltage Von of the MOSFET before the body diode is energized (at room temperature) is measured (step S3). In the process of step S3, the drain-source voltage Vds0 of the MOSFET before the body diode is energized is measured as the on-voltage Von of the MOSFET. The measurement variability of the drain-source voltage Vds of the MOSFET is smaller than the measurement variability of the forward voltage Vf of the body diode (see Figures 4 to 6). For this reason, by measuring the drain-source voltage Vds of the MOSFET as the on-voltage Von of the MOSFET, it is possible to improve screening accuracy.
[0049] Specifically, with a gate voltage Vg (e.g., Vg = +15V) equal to or greater than the gate threshold voltage applied to the gate pad, an on-signal of a Von measurement pulse signal (Fig. 3(d)) of a prescribed strength is input between the source pad 14 and the drain electrode 15 via the probe, and a prescribed drain-source current Ids (set current) is passed through the MOSFET for the duration of the on-signal of the Von measurement pulse signal (on-pulse width). The drain-source voltage Vds0 of the MOSFET at this time is measured, and this drain-source voltage Vds0 is obtained as the on-voltage Von of the MOSFET before the body diode is energized.
[0050] The Von measurement pulse signal may be either a single pulse or a continuous pulse, as long as it is turned on at the off timing of the BD current pulse signal and the off timing of the temperature measurement pulse signal. When the Von measurement pulse signal is a single pulse, an on signal for one period of the Von measurement pulse signal is input at a predetermined timing. When the Von measurement pulse signal is a continuous pulse, the Von measurement pulse signal is turned on (on signal input) and off (off signal input) continuously for a predetermined period. Figure 3(d) shows a state in which an on signal of the Von measurement pulse signal is input at a predetermined timing (single pulse).
[0051] When a current sense of the main element is provided on the semiconductor substrate 30, a Von measurement pulse signal may be input to the current sense via a sense probe, and the drain-source voltage Vds of the current sense may be acquired as the on-voltage Von of the main element. In this case, a BD energization pulse signal and a temperature measurement pulse signal are input to the main element via the remaining probes excluding the sense probe. For this reason, the on-timing of the Von measurement pulse signal may overlap with the on-timing of the BD energization pulse signal and the on-timing of the temperature measurement pulse signal, improving the degree of freedom in design.
[0052] The strength (amplitude) of the Von measurement pulse signal is set to a strength that causes the rated drain-source current Ids to flow through the MOSFET when the Von measurement pulse signal is input as an on signal. Specifically, the strength of the Von measurement pulse signal is, for example, such that the drain-source current Ids flowing through the MOSFET when the Von measurement pulse signal is input as an on signal is 1 A or more. Also, the strength of the Von measurement pulse signal is, for example, equal to or less than a strength that obtains a drain-source voltage Vds0 that is approximately the same voltage value as the forward voltage Vf of the body diode when the set current by the BD current-carrying pulse signal flows.
[0053] Next, input of the BD energization pulse signal (FIG. 3(a)) is started to start energizing the body diode (step S4). The BD energization pulse signal is a continuous pulse that is continuously turned on (on signal input) and off (off signal input) at a predetermined cycle. The on timing of the temperature measurement pulse signal (FIG. 3(c)) and the on timing of the Von measurement pulse signal (FIG. 3(d)) are set so that they do not overlap with the on signal input of the BD energization pulse signal. The strength of the BD energization pulse signal is set to, for example, such that the forward current If flowing through the body diode in response to the on signal input of the temperature measurement pulse signal is 20 A or more and less than the rated current.
[0054] Specifically, with no gate voltage applied to the gate pad or with a negative gate voltage Vg applied to the gate pad via the probe to turn off the MOSFET, an ON signal of a BD energization pulse signal of a predetermined strength is input between the source pad 14 and the drain electrode 15 via the probe, and a predetermined forward current If (set current) flows through the body diode for the duration of the ON signal of the BD energization pulse signal (ON pulse width). This causes the semiconductor substrate 30 to generate heat, and the temperature Tm of the semiconductor substrate 30 to rise to a temperature according to the forward current If of the body diode.
[0055] Therefore, the temperature Tm of the semiconductor substrate 30 is calculated, and it is confirmed whether the temperature Tm of the semiconductor substrate 30 is a set temperature (maximum temperature) T1 according to the strength of the BD energization pulse signal. At this time, the temperature Tm of the semiconductor substrate 30 is calculated in the same manner and under the same conditions as before the body diode is energized. Specifically, an on signal of the temperature measurement pulse signal is input under the same conditions as before the body diode is energized to pass a predetermined forward current If (set current) through the body diode, and the forward voltage Vf of the body diode at this time is measured, and this forward voltage Vf is obtained as the voltage Vm1 applied to the semiconductor substrate 30 at the beginning of energization of the body diode (at high temperature).
[0056] The temperature Tm1 of the semiconductor substrate 30 at the beginning of the conduction of the body diode is calculated one or more times using the voltage Vm1 applied to the semiconductor substrate 30 at the beginning of the conduction of the body diode, the temperature Tm0 of the semiconductor substrate 30 before the conduction of the body diode, the voltage Vm0 applied to the semiconductor substrate 30, and the above formula (1). When the temperature Tm1 of the semiconductor substrate 30 reaches the set temperature T1, the on-voltage Von of the MOSFET is measured (step S5). In the process of step S5, the drain-source voltage Vds1 of the MOSFET at the beginning of the conduction of the body diode is measured in the same manner and under the same conditions as the process of step S3.
[0057] Next, after a predetermined time for energizing the body diode has elapsed, the voltage Vm1 applied to the semiconductor substrate 30 is measured immediately before the end of energizing the body diode, and the temperature Tm1 of the semiconductor substrate 30 is calculated. The measurement of the voltage Vm1 applied to the semiconductor substrate 30 and the calculation of the temperature Tm1 of the semiconductor substrate 30 at this time are performed in the same manner and under the same conditions as the measurement of the voltage Vm1 applied to the semiconductor substrate 30 and the calculation of the temperature Tm1 of the semiconductor substrate 30 immediately before step S5, respectively. Next, the on-voltage Von of the MOSFET is measured (step S6). In the process of step S6, the drain-source voltage Vds1 of the MOSFET immediately before the end of energizing the body diode is measured in the same manner and under the same conditions as step S5.
[0058] Next, the input of the BD energization pulse signal is terminated to terminate energization of the body diode (step S7). Since the semiconductor substrate 30 no longer generates heat by terminating energization of the body diode, the semiconductor substrate 30 is left as is to cool down to room temperature (step S8). Next, the temperature Tm of the semiconductor substrate 30 is calculated, and it is confirmed whether the temperature Tm of the semiconductor substrate 30 has reached room temperature (the stage temperature T0 before energization of the body diode). That is, an ON signal of the temperature measurement pulse signal is input under the same conditions as before energization of the body diode, and the forward voltage Vf of the body diode is obtained as the voltage Vm2 applied to the semiconductor substrate 30 after energization of the body diode (at room temperature).
[0059] The temperature Tm2 of the semiconductor substrate 30 after the body diode is energized is calculated one or more times using the voltage Vm2 applied to the semiconductor substrate 30 after the body diode is energized, the temperature Tm0 of the semiconductor substrate 30 before the body diode is energized, and the voltage Vm0 applied to the semiconductor substrate 30, and an equation in which Vm1 in equation (1) is replaced with Vm2. When the temperature Tm2 of the semiconductor substrate 30 becomes room temperature (i.e., when Tm2=T0), the on-voltage Von of the MOSFET after the body diode is energized is measured (step S9). In the process of step S9, the drain-source voltage Vds2 of the MOSFET after the body diode is energized is measured in the same manner and under the same conditions as in the process of step S3.
[0060] Next, input of the temperature measurement pulse signal (FIG. 3(c)) is terminated (step S10). Next, the amount of fluctuation (Von fluctuation) ΔVon of the on-voltage Von of the MOSFET is calculated (step S11). In the process of step S11, the amount of fluctuation ΔVon of the on-voltage Von of the MOSFET is calculated under two conditions: when the temperature Tm of the semiconductor substrate 30 is a high temperature, which is the set temperature T1 when the body diode is energized, and when it is room temperature (stage temperature T0 before the body diode is energized). Specifically, the amount of fluctuation ΔVon of the on-voltage Von of each MOSFET at high temperature and at room temperature is calculated using the following formulas (2) and (3), respectively.
[0061] ΔVon (at high temperature) = Vds1_1-Vds1_2 ···(2)
[0062] ΔVon (at room temperature) = Vds2 - Vds0 (3)
[0063] In the above equation (2), ΔVon (at high temperature) is the amount of fluctuation in the MOSFET on-voltage Von at high temperature (set temperature T1). The set temperature T1 is, for example, 150°C or higher. Vds1_1 and Vds1_2 are the MOSFET on-voltage Von (drain-source voltage Vds) at the beginning of current flow through the body diode and immediately before current flow ends, respectively. In the above equation (3), ΔVon (at room temperature) is the amount of fluctuation in the MOSFET on-voltage Von at room temperature. Vds0 and Vds2 are the MOSFET on-voltage Von (drain-source voltage Vds) before and after current flow through the body diode, respectively.
[0064] The variation ΔVon of the on-voltage Von of the MOSFET at high temperature and room temperature is calculated using the above formula (2) and formula (3), respectively. By screening (selecting) semiconductor substrates 30 that have no variation in the on-voltage Von of the MOSFET at high temperature and room temperature, silicon carbide semiconductor devices 10 in which stacking faults have not grown can be screened as good products. "No variation in the on-voltage Von of the MOSFET" refers to a case in which the variation ΔVon of the on-voltage Von of the MOSFET at high temperature is about ±1% or less, and the variation ΔVon of the on-voltage Von of the MOSFET at room temperature is about ±2% or less.
[0065] The semiconductor substrate 30 may be screened based only on the amount of variation ΔVon of the on-voltage Von of the MOSFET at high temperature. In this embodiment, the semiconductor substrate 30 can be screened based on two judgment factors, the amount of variation ΔVon of the on-voltage Von of the MOSFET at high temperature and the amount of variation ΔVon of the on-voltage Von of the MOSFET at room temperature. The inventors' intensive research has confirmed that the screening accuracy of the semiconductor substrate 30 is improved by increasing the number of judgment factors for screening. Thereafter, the probe is removed from the semiconductor chip (step S12), and the screening inspection of the semiconductor substrate 30 is completed.
[0066] Since the above-mentioned processes from step S1 (connecting the probe to the semiconductor substrate 30) to step S12 (removing the probe from the semiconductor substrate 30) can be performed by one inspection device, an increase in the number of steps in the screening inspection can be suppressed. Also, the fluctuation in the on-voltage Von of the MOSFET can be grasped almost simultaneously with the end of conduction of current through the body diode. Furthermore, in the inspection method for silicon carbide semiconductor device 10 according to the above-mentioned embodiment, the process of step S9 and the process of step S10 may be interchanged. Also, the process of step S11 and the process of step S12 may be interchanged.
[0067] In addition, in the process of step S11, the calculation of the variation ΔVon of the on-voltage Von of the MOSFET at high temperature may be performed at any time after the process of step S6 (measuring the drain-source voltage Vds1 (on-voltage Von) of the MOSFET immediately before the end of current flow through the body diode). In the process of step S11, the calculation of the variation ΔVon of the on-voltage Von of the MOSFET at room temperature may be performed at any time after the process of step S9 (measuring the drain-source voltage Vds2 (on-voltage Von) of the MOSFET after current flow through the body diode).
[0068] Furthermore, between the process of step S5 and the process of step S6 (while the body diode is conducting), a set of steps including calculating the temperature Tm1 of the semiconductor substrate 30, measuring the voltage Vm1 applied to the semiconductor substrate 30 at the temperature Tm1 of the semiconductor substrate 30, and measuring the drain-source voltage Vds1 (on-voltage Von) of the MOSFET may be performed one or more times. In this case, the amount of change ΔVon in the on-voltage Von of the MOSFET at high temperature may be calculated using the drain-source voltage Vds1 of any of the MOSFETs measured while the body diode is conducting in the above formula (2).
[0069] The stage, probe, measuring device, and the like of the inspection device are controlled by a control means (not shown). Moreover, the inspection method for a silicon carbide semiconductor device (semiconductor substrate 30) according to this embodiment can be realized by executing a prepared program on a computer such as a personal computer or a workstation, a database server, or a web server. The inspection results and detection results obtained by executing this program, and information previously obtained for obtaining these inspection results and detection results, are stored in a computer-readable storage medium (not shown).
[0070] Furthermore, the voltage waveforms of the voltages Vm0, Vm1, Vm2 (forward voltage Vf of the body diode) applied to the semiconductor substrate 30 measured during the period from step S1 to step S12 described above may be output to a display means such as a monitor so as to be constantly observable. The voltage waveforms of the MOSFET on-voltages Von (MOSFET drain-source voltages Vds0, Vds1, Vds2) measured during the period from step S1 to step S12 described above may be output to a display means different from the voltage waveforms of the voltages Vm0, Vm1, Vm2 applied to the semiconductor substrate 30 so as to be constantly observable.
[0071] This program is recorded on a computer-readable recording medium and executed by being read from the recording medium by a computer or a server. The recording medium may be a solid state drive (SSD), a hard disk drive (HDD), a Blu-ray (registered trademark) Disc (BD), a flexible disk, a USB flash memory, a CD-ROM, an MO, a DVD, etc. This program may also be a transmission medium that can be distributed via a network such as the Internet.
[0072] As described above, according to the embodiment, after starting the conduction of the body diode by inputting a BD conduction pulse signal of a predetermined period, and before terminating the conduction of the body diode by terminating the input of the BD conduction pulse signal, the drain-source voltage of the MOSFET is measured at least twice at different timings for the heated semiconductor chip. Then, screening is performed based on the difference (variation: determination factor) between the measured drain-source voltages. Since screening is performed based on the drain-source voltage of the MOSFET, which has smaller measurement variation compared to the forward voltage of the body diode, screening accuracy can be improved compared to the case of screening based on the forward voltage of the body diode.
[0073] Moreover, according to the embodiment, the drain-source voltage of the MOSFET is measured at room temperature before and after current is passed through the body diode, and screening is performed based on the difference between the measured values. By performing screening based on judgment factors obtained for semiconductor chips at different temperatures, the screening accuracy can be further improved. Furthermore, according to the embodiment, a set of input terminals (probes) for passing current through the body diode is used to measure the drain-source voltage of the MOSFET while the body diode is passing current (and also before and after passing current), and judgment factors for screening can be obtained almost simultaneously with the end of current passing through the body diode. This makes it possible to reduce the number of steps in the screening test.
[0074] Moreover, according to the embodiment, by passing a forward current through the body diode by inputting a BD energization pulse signal, the duration of the off signal of the BD energization pulse signal (off pulse width) can be set to a time during which no forward current flows through the body diode even if a forward current of high current density flows through the body diode. This makes it possible to prevent the semiconductor chip from being overheated. Furthermore, according to the embodiment, during the period from when the probe is pressed against the semiconductor substrate to when it is released, it is possible to conduct the body diode and measure the voltage, which is a judgment factor for screening. This makes it possible to suppress changes in contact resistance caused by the probe due to the conduction of the body diode and the screening test.
[0075] (Experimental Example) We investigated the relationship between the measurement variability of the drain-source voltage Vds of a MOSFET and the presence or absence of stacking fault growth. Figure 4 is a characteristic diagram showing the measurement variability of the drain-source voltage of a MOSFET at room temperature in an experimental example. Figure 5 is a characteristic diagram showing the measurement variability of the drain-source voltage of a MOSFET at high temperature (set temperature T1 = 175°C) in an experimental example. Figure 6 is a characteristic diagram showing the measurement variability of the forward voltage of the body diode of the comparative example.
[0076] In Figure 4, the horizontal and vertical axes respectively show the drain-source voltage Vds of the MOSFET before and after the body diode is energized (before BD is energized and after BD is energized).In Figure 5, the horizontal and vertical axes respectively show the drain-source voltage Vds of the MOSFET at the beginning of body diode energization and just before the end of energization (at the beginning of BD energization and just before BD is energized).In Figure 6, the horizontal and vertical axes respectively show the forward voltage Vf before and after the body diode is energized.
[0077] According to the inspection method for silicon carbide semiconductor device 10 according to the embodiment described above, the drain-source voltage Vds of the MOSFET was measured at room temperature and at a high temperature for a plurality of semiconductor substrates (semiconductor chips) 30 (hereinafter referred to as experimental examples), and the results are shown in Figures 4 and 5. Each sample in the experimental examples has a different strength of the Von measurement pulse signal for measuring the drain-source voltage Vds of the MOSFET.
[0078] Figure 4 shows, with a solid line, the baseline when the drain-source voltage Vds does not fluctuate before and after the passage of current through the body diode. Figure 5 shows, with a solid line, the baseline when the drain-source voltage Vds does not fluctuate at the beginning of current passage through the body diode and just before the end of current passage. Figures 4 and 5 also show, with dashed lines, the ranges when the deviation from the baseline is ±2% and ±1%, respectively, as the pass ranges for screening. The pass range for screening is the allowable range of measurement variation, and is the range within which it is determined that no stacking faults have grown in the screening inspection.
[0079] Moreover, the results of measuring the forward voltage Vf before and after energization of the body diode for a number of semiconductor substrates 30 (hereinafter referred to as comparative examples) are shown in Fig. 6. Each comparative example sample has a different strength of the BD energization pulse signal for energizing the body diode. In Fig. 6, a solid line indicates a reference line for when the forward voltage Vf does not vary before and after energization of the body diode, and a dashed line indicates a range for when the forward voltage Vf varies by ±5% from the reference line as the pass range for screening.
[0080] From the results of the experimental example shown in Figure 4, it was confirmed that the acceptable range of the drain-source voltage Vds of a MOSFET at room temperature can be set within ±2% of the reference line. Sample 41, in which the drain-source voltage Vds of the MOSFET at room temperature falls outside the allowable range, can be determined to be a sample in which the drain-source voltage Vds of the MOSFET has fluctuated. It was confirmed that stacking faults have grown in this sample 41.
[0081] From the results of the experimental example shown in Figure 5, it was confirmed that the acceptable range of the drain-source voltage Vds of a MOSFET at high temperatures can be set to within ±1% from the reference line. Sample 42, in which the drain-source voltage Vds of the MOSFET at high temperatures falls outside the allowable range, can be determined to be a sample in which the drain-source voltage Vds of the MOSFET has fluctuated. It was confirmed that stacking faults have grown in this sample 42.
[0082] The reason that the pass range of the MOSFET drain-source voltage Vds can be narrowed at high temperatures compared to room temperature is because the absolute value of the MOSFET drain-source voltage Vds is larger at high temperatures compared to room temperature. Because the absolute value of the MOSFET drain-source voltage Vds is small at room temperature, the amount of fluctuation in the MOSFET drain-source voltage Vds before and after the body diode is conductive is large.
[0083] In addition, from the results of the comparative example shown in Figure 6, it was confirmed that the measurement variability of the forward voltage Vf before and after current flow through the body diode tends to be larger than the measurement variability of the drain-source voltage Vds of the MOSFET at room temperature and at high temperatures (see Figures 4 and 5). The reason for this is presumed to be as follows. The drain-source voltage Vds of a MOSFET is determined by the ++ This is independent of temperature changes in the contact region 6 (see FIG. 1(a)).
[0084] In contrast, the forward voltage Vf of the body diode is ++This is presumably because the forward voltage Vf depends on the contact resistance of the contact region 6 (see FIG. 1(b)), and this contact resistance changes with an increase in temperature of the semiconductor substrate 30. In addition, in the comparative examples, many of the samples showed a tendency for the forward voltage Vf to increase after the body diode was energized, but the growth of stacking faults was not confirmed in any of the samples.
[0085] Furthermore, in the comparative example, no growth of stacking faults was observed even in samples in which the forward voltage Vf after the body diode was energized varied by more than +5% from the reference line. Therefore, from the results shown in Figures 4 to 6, it was confirmed that by comparing the drain-source voltage Vds of the MOSFET before and after the body diode is energized, it is possible to improve the screening accuracy more than by comparing the forward voltage Vf after the body diode is energized.
[0086] In the experimental example described above, the pass ranges for the drain-source voltage Vds of a MOSFET that is determined to be a pass product in the screening test were set to within ±2% and ±1% at room temperature and high temperature, respectively. However, the range of measurement variation in the drain-source voltage Vds of a MOSFET that is determined to be a pass product in this screening test is variously set depending on the design conditions of silicon carbide semiconductor device 10.
[0087] The present invention is not limited to the above-mentioned embodiment, and various modifications are possible without departing from the spirit of the present invention. For example, in the above-mentioned embodiment, the MOSFET on-voltage Von (drain-source voltage Vds) is measured four times (before the body diode is energized, at the beginning of energization, immediately before the end of energization, and after energization) but the present invention is not limited to this, and the MOSFET on-voltage Von may be measured at a different timing during the body diode energization in addition to the four timings described above.
[0088] Also, for example, in the above-mentioned embodiment, the dimensions and impurity concentration of each part of the silicon carbide semiconductor device, the conditions of the pulse signal input to the silicon carbide semiconductor device (amplitude, period, pulse width), etc. are variously set according to the required specifications, etc. Also, in the above-mentioned embodiment, the case where silicon carbide is used as the wide band gap semiconductor is described as an example, but the present invention is also applicable to wide band gap semiconductors other than silicon carbide, such as gallium nitride (GaN). Also, the present invention is similarly valid when the conductivity type (n-type, p-type) is reversed. [Industrial Applicability]
[0089] As described above, the method for inspecting a silicon carbide semiconductor device according to the present invention is useful for inspecting a silicon carbide semiconductor device in which a parasitic pn diode (body diode) is formed by a pn junction inside a semiconductor substrate, and is particularly suitable for inspecting MOSFETs. [Explanation of symbols]
[0090] 1n + Type drain region 2a n-type buffer region 2b n - Mold Drift Region 3 n-type current diffusion region 4 p-type base region 5n ++ Type Source Area 6 p ++ Mold Contact Area 7. Trench 8 Gate insulating film 9 Gate electrode 10 Silicon carbide semiconductor device 11 Interlayer insulating film 12 Barrier metal 13 Source electrode 14 Sauce Pad 15 Drain electrode 21,22 p + type area 23n + type area 30 Semiconductor substrate (semiconductor chip) 31 n+ Starting substrate 32 n-type epitaxial layer 33n - Type epitaxial layer 34 p-type epitaxial layer
Claims
1. A semiconductor chip made of silicon carbide; a first semiconductor region of a first conductivity type provided inside the semiconductor chip; a second semiconductor region of a second conductivity type provided between a front surface of the semiconductor chip and the first semiconductor region; a third semiconductor region of a first conductivity type selectively provided between a front surface of the semiconductor chip and the second semiconductor region; a gate insulating film provided in contact with a region of the second semiconductor region between the third semiconductor region and the first semiconductor region; a gate electrode provided on the opposite side of the second semiconductor region with the gate insulating film interposed therebetween; a first electrode electrically connected to the second semiconductor region and the third semiconductor region; A method for inspecting a silicon carbide semiconductor device comprising: a first step of energizing a parasitic diode formed by a pn junction between the second semiconductor region and the first semiconductor region by inputting a first pulse signal having a predetermined period; a second step of flowing a predetermined first current from the second electrode to the first electrode in the semiconductor chip by inputting an on-signal of a predetermined second pulse signal, and measuring a positive first voltage applied to the second electrode with respect to the first electrode; a third step of terminating the input of the first pulse signal to terminate the conduction of the parasitic diode; a fourth step of calculating a first difference between two of the first voltages obtained by performing the second step at different timings on the semiconductor chip that has generated heat in the first step after the first step and before the third step; a fifth step of selecting the semiconductor chips having the first difference within a first predetermined range as non-defective products; 2. A method for inspecting a silicon carbide semiconductor device comprising:
2. A sixth step of calculating a second difference between the first voltage obtained by performing the second step on the semiconductor chip before the first step and the first voltage obtained by performing the second step on the semiconductor chip whose temperature has been reduced after the third step, 2. The method for inspecting a silicon carbide semiconductor device according to claim 1, wherein in the sixth step, the semiconductor chips for which the first difference is within the first predetermined range and the second difference is within a second predetermined range are selected as non-defective products.
3. 3. The method for inspecting a silicon carbide semiconductor device according to claim 1, wherein in the fourth step, the first difference between the first voltage acquired by performing the second step at an early stage of current flow through the parasitic diode and the first voltage acquired by performing the second step after a predetermined current flow time of the parasitic diode has elapsed is calculated.
4. a seventh step of flowing a second current in a forward direction through the parasitic diode by inputting a third pulse signal as an on-signal, and measuring a second positive voltage applied to the first electrode relative to the second electrode; an eighth step of calculating a temperature of the semiconductor chip based on the second voltage; Further comprising:
4. The method for inspecting a silicon carbide semiconductor device according to claim 1, wherein the temperature of the semiconductor chip is acquired by the seventh step and the eighth step, and the second step is performed after confirming that the temperature of the semiconductor chip is a predetermined set temperature.
5. In the seventh step, the second voltage is measured when the second current, which is 1 / 1000 of the rated current of the parasitic diode, is caused to flow through the parasitic diode; 5. The method for inspecting a silicon carbide semiconductor device according to claim 4, characterized in that in the eighth step, a temperature of the semiconductor chip is calculated based on the second voltage obtained by performing the seventh step before the first step and the second voltage obtained by performing the seventh step after the first step.
6. 6. The method for inspecting a silicon carbide semiconductor device according to claim 4 or 5, wherein in the seventh step, an on signal of the third pulse signal is input at a timing different from that of the on signal input of the first pulse signal and the second pulse signal.
7. 7. The method for inspecting a silicon carbide semiconductor device according to claim 1, wherein, in the second step, an on signal of the second pulse signal is input at a timing different from that of the on signal input of the first pulse signal.
Citation Information
Patent Citations
Inspecting method and apparatus for silicon carbide semiconductor device, and manufacturing method for silicon carbide semiconductor device
JP2004289023A
Method and device for inspecting silicon carbide semiconductor device
JP2015065250A
Semiconductor device
JP2019054064A
Selecting method of silicon carbide semiconductor device