Colored composition, color filter substrate using the same, method for producing the same, and display device

A coloring composition with dipentaerythritol hexa(meth)acrylate and pentaerythritol tri(meth)acrylate addresses pattern peeling and color mixing issues in color filter substrates, ensuring stability and purity at low firing temperatures, suitable for silicon OLEDs and electronic paper.

JP7593126B2Active Publication Date: 2024-12-03TORAY INDUSTRIES INC
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2021006155
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-01-21
Filing Date
2021-01-19
Publication Date
2024-12-03
Estimated Expiration
2041-01-19

AI Technical Summary

Technical Problem

Existing coloring compositions for color filter substrates face issues with pattern peeling, color mixing, and pin unevenness when fired at low temperatures, particularly in applications like silicon OLEDs and electronic paper, where high temperatures are not feasible.

Method used

A coloring composition comprising dipentaerythritol hexa(meth)acrylate and pentaerythritol tri(meth)acrylate with specific weight ratios, along with a photopolymerization initiator and organic solvent, is used to form a color filter substrate through exposure and development, ensuring pattern stability and color purity even at low firing temperatures.

Benefits of technology

The composition effectively prevents pattern peeling and color mixing, maintaining color purity and stability during low-temperature processing, suitable for applications like silicon OLEDs and electronic paper.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007593126000001
    Figure 0007593126000001
  • Figure 0007593126000002
    Figure 0007593126000002
  • Figure 0007593126000003
    Figure 0007593126000003
Patent Text Reader

Abstract

To provide a color filter substrate using a coloring composition which prevents pattern peeling in overcoating processing even when being baked at low temperature, can suppress color mixture of a pattern, and prevents pin unevenness.SOLUTION: A coloring composition contains a colorant, a binder resin, a radical polymerizable compound, a photopolymerization initiator and an organic solvent. The radical polymerizable compound contains dipentaerythritol hexa(meth)acrylate and pentaerythritol tri(meth)acrylate, a ratio of a weight (A) of the dipentaerythritol hexa(meth)acrylate to a weight (B) of the pentaerythritol tri(meth)acrylate is 0.16<A / B<3, and a ratio of a weight (P) of a component excluding the colorant, the radical polymerizable compound, the photopolymerization initiator and the organic solvent to a weight (R) of the radical polymerizable compound is 0.5<P / R<1.2.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a colored composition, a color filter substrate using the same, a method for producing the same, and a display device. [Background technology]

[0002] Taking advantage of their characteristics such as light weight, thinness, and low power consumption, liquid crystal display devices are used in various applications such as televisions, notebook computers, personal digital assistants, smartphones, digital cameras, etc. Liquid crystal display devices are required to have optimal colors out of three to six primary colors depending on the application, and color filter substrates that provide various color performance are used.

[0003] Color filter substrates are generally manufactured by performing exposure and development when forming colored pixels, and then baking at a temperature of 200° C. or higher. On the other hand, in color filter type electronic paper and silicon OLED, etc., colored pixels are formed on a film or light emitting element, so baking at a temperature of 100° C. or lower is required to prevent deterioration of the film or light emitting element.

[0004] Coloring compositions containing epoxy compounds are known as coloring compositions for color filters (see, for example, Patent Document 1, Patent Document 2, and Patent Document 3). When an epoxy compound is added, crosslinking due to thermal curing proceeds, and even if the baking temperature is low, color mixing of pixels is unlikely to occur during color filter formation. However, there are problems with insufficient color mixing suppression and storage stability, and improvements have been required. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2011-22371 A [Patent Document 2] JP 2012-212051 A [Patent Document 3] International Publication No. 2015 / 182285 Summary of the Invention [Problem to be solved by the invention]

[0006] An object of the present invention is to provide a coloring composition which is unlikely to cause pattern peeling during overcoating processing even when baked at a low temperature, can suppress color mixing of patterns, and is unlikely to cause pin unevenness, and to provide a color filter substrate and a display device which use such a coloring composition. [Means for solving the problem]

[0007] In order to solve the above problems, the coloring composition of the present invention has the following configuration. A coloring composition comprising a coloring material, a binder resin, a radical polymerizable compound, a photopolymerization initiator and an organic solvent, wherein the radical polymerizable compound comprises dipentaerythritol hexa(meth)acrylate and pentaerythritol tri(meth)acrylate, and the ratio of the weight (A) of the dipentaerythritol hexa(meth)acrylate to the weight (B) of the pentaerythritol tri(meth)acrylate is 0.16

[0008] The color filter substrate of the present invention has the following configuration. and a color filter substrate having pixels formed of a photocured product of the coloring composition.

[0009] The method for producing a color filter substrate of the present invention has the following configuration. The method for producing a color filter substrate includes the steps of (A) applying the above-mentioned coloring composition onto a substrate, (B) forming a pattern by exposure and development, and (C) further exposing the formed pattern to light.

[0010] ​The display device of the present invention has the following configuration. That is, it is a display device having the above color filter substrate.

[0011] The coloring composition of the present invention preferably further contains a photosensitizer.

[0012] In the coloring composition containing a photosensitizer which is a preferred embodiment of the present invention, the ratio of the weight (P) of the components excluding the colorant, radical polymerizable compound, photopolymerization initiator, organic solvent, and photosensitizer to the weight (R) of the radical polymerizable compound is more preferably 0.5 < P / R < 1.2.

[0013] In the coloring composition of the present invention, it is preferable that the number of moles M of double bonds contained per gram of solid content T excluding the colorant satisfies 160 < T / M < 220.

[0014] In the coloring composition of the present invention, it is preferable that the colorant includes a diketopyrrolopyrrole pigment having a bromine group.

[0015] In the coloring composition of the present invention, it is preferable that the photosensitizer is a thioxanthone-based sensitizer.

[0016] In the coloring composition of the present invention, it is preferable that the ratio of the weight (K) of the photosensitizer to the weight (L) of the photopolymerization initiator is 0.3 < K / L < 0.6.

[0017] In the coloring composition of the present invention, it is preferable that the total content of dipentaerythritol hexa(meth)acrylate and pentaerythritol tri(meth)acrylate in the radical polymerizable compound is 70% by mass or more.

Advantages of the Invention

[0018] According to the coloring composition of the present invention, even when fired at a low temperature, pattern peeling during overcoating is less likely to occur, and furthermore, color mixing of the pattern can be suppressed, and a coloring composition in which pinholes are less likely to occur can be provided.

Embodiments for Carrying Out the Invention

[0019] The coloring composition of the present invention is a coloring composition containing a colorant, a binder resin, a radical polymerizable compound, a photopolymerization initiator and an organic solvent, wherein the radical polymerizable compound contains dipentaerythritol hexa(meth)acrylate and pentaerythritol tri(meth)acrylate, and the ratio of the weight (A) of the dipentaerythritol hexa(meth)acrylate to the weight (B) of the pentaerythritol tri(meth)acrylate is 0.16

[0020] The coloring composition of the present invention contains a coloring material. Examples of the coloring material include organic pigments, inorganic pigments, dyes, etc., and two or more of these may be contained. Among these, organic pigments and dyes are preferred from the viewpoint of further improving the transmittance.

[0021] Examples of red colorants include CI Pigment Red (hereinafter, "PR") 9, PR48, PR97, PR122, PR123, PR144, PR149, PR166, PR168, PR177, PR179, PR180, PR192, PR209, PR215, PR216, PR217, PR220, PR223, PR224, PR226, PR227, PR228, PR240, PR254, and diketopyrrolopyrrole colorants having a bromine group. From the viewpoint of pixel brightness characteristics, PR254, PR177, and diketopyrrolopyrrole colorants having a bromine group are preferred, and from the viewpoints of brightness, vividness, and prevention of color mixing, it is preferred to use a diketopyrrolopyrrole colorant having a bromine group.

[0022] ​Examples of yellow colorants include organic pigments, inorganic pigments, dyes, and the like, such as CI Pigment Yellow (hereinafter referred to as "PY") 12, PY13, PY17, PY20, PY24, PY83, PY86, PY93, PY95, PY109, PY110, PY117, PY125, PY129, PY137, PY139, PY147, PY148, PY150, PY153, PY154, PY166, and PY168 (all numbers are color index numbers). Two or more of these may be contained. From the viewpoints of color purity, light transmittance, and contrast, PY129, PY139, PY150, and PY185 are preferred, and PY150 and PY185 are more preferred.

[0023] Examples of green colorants include organic pigments, inorganic pigments, dyes, etc., such as CI Pigment Green (hereinafter referred to as "PG") PG1, PG2, PG4, PG7, PG8, PG10, PG13, PG14, PG15, PG17, PG18, PG19, PG26, PG36, PG38, PG39, PG45, PG48, PG50, PG51, PG54, PG55, PG58, PG59 (all numbers are color index numbers), etc. Two or more of these may be contained.

[0024] Examples of orange colorants include CI Pigment Orange (hereinafter, "PO") 13, PO31, PO36, PO38, PO40, PO42, PO43, PO51, PO55, PO59, PO61, PO64, PO65, and PO71.

[0025] Examples of blue colorants include CI Pigment Blue (hereinafter, "PB") 15, PB15:3, PB15:4, PB15:6, PB21, PB22, PB60, and PB64.

[0026] Examples of purple colorants include CI Pigment Violet (hereinafter referred to as "PV") 19, PV23, PV29, PV30, PV32, PV37, PV40, and PV50 (all numbers are Color Index Nos.).

[0027] Examples of the dye include oil-soluble dyes, acid dyes, direct dyes, basic dyes, acid mordant dyes, etc. The dyes may be made into lakes or may be made into salts of the dyes and nitrogen-containing compounds.

[0028] Examples of red, green, blue, purple or yellow dyes include direct dyes, acid dyes, and basic dyes. Specific examples of these dyes include azo dyes, benzoquinone dyes, naphthoquinone dyes, anthraquinone dyes, xanthene dyes, cyanine dyes, squarylium dyes, croconium dyes, merocyanine dyes, stilbene dyes, diarylmethane dyes, triarylmethane dyes, fluoran dyes, spiropyran dyes, phthalocyanine dyes, indigo dyes, fulgide dyes, nickel complex dyes, and azulene dyes. The dye may be dissolved in the coloring composition or dispersed as particles.

[0029] In order to enhance resistance to heat, light, acid, alkali, organic solvents, etc., the basic dye is preferably a salt-forming compound made of an organic acid such as an organic sulfonic acid or an organic carboxylic acid, or perchloric acid, and more preferably a salt-forming compound made of a naphthalenesulfonic acid such as Tobias acid, or perchloric acid. Similarly, in order to enhance resistance to heat, light, acid, alkali, organic solvents, etc., the acid dye and direct dye are preferably a salt-forming compound made of a quaternary ammonium salt, primary to tertiary amine, or sulfonamide.

[0030] The coloring composition of the present invention contains a binder resin. By containing the binder resin, it is possible to suppress unevenness in the film thickness during film formation and to suppress deformation of the pattern due to flow during firing.

[0031] Examples of the binder resin include acrylic resin, epoxy resin, polyimide resin, urethane resin, urea resin, polyvinyl alcohol resin, melamine resin, polyamide resin, polyamideimide resin, polyester resin, polyolefin resin, etc. Two or more of these may be contained. From the viewpoint of stability, acrylic resin is preferably used.

[0032] The acrylic resin is preferably a copolymer of an unsaturated carboxylic acid and an ethylenically unsaturated compound.

[0033] Examples of the unsaturated carboxylic acid include acrylic acid, methacrylic acid, itaconic acid, crotonic acid, maleic acid, fumaric acid, vinylacetic acid, and acid anhydrides thereof. Two or more of these may be used.

[0034] Examples of the ethylenically unsaturated compounds include unsaturated carboxylic acid alkyl esters such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, sec-butyl (meth)acrylate, iso-butyl (meth)acrylate, tert-butyl (meth)acrylate, n-pentyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, and benzyl (meth)acrylate; aromatic vinyl compounds such as styrene, p-methylstyrene, o-methylstyrene, m-methylstyrene, and α-methylstyrene; and aminoethyl Examples of the monomer include unsaturated carboxylic acid amino alkyl esters such as acrylate, unsaturated carboxylic acid glycidyl esters such as glycidyl acrylate and glycidyl methacrylate, carboxylic acid vinyl esters such as vinyl acetate and vinyl propionate, cyanide vinyl compounds such as acrylonitrile, methacrylonitrile and α-chloroacrylonitrile, aliphatic conjugated dienes such as 1,3-butadiene and isoprene, and macromonomers such as polystyrene having a (meth)acryloyl group at the end, polymethyl acrylate, polymethyl methacrylate, polybutyl acrylate, polybutyl methacrylate, and polysilicone. Two or more of these may be used.

[0035] The acrylic resin preferably has an ethylenically unsaturated group in the side chain, which can improve sensitivity. Examples of the ethylenically unsaturated group include vinyl groups, allyl groups, acrylic groups, and methacrylic groups. Examples of the acrylic resin having an ethylenically unsaturated group in the side chain include "Cyclomer" (registered trademark) P (Daicel Chemical Industries, Ltd.) and alkali-soluble cardo resins.

[0036] The weight average molecular weight of the binder resin is preferably 3,000 or more, more preferably 9,000 or more, from the viewpoint of the strength of the cured film. On the other hand, from the viewpoint of the stability of the coloring composition, the weight average molecular weight of the binder resin is preferably 200,000 or less, more preferably 100,000 or less. Here, the weight average molecular weight of the binder resin refers to a standard polystyrene equivalent value measured by gel permeation chromatography.

[0037] From the viewpoint of suppressing unevenness in the thickness during film formation, the content of the binder resin is preferably 10% by mass or more, more preferably 20% by mass or more, and even more preferably 30% by mass or more, based on the solid content. On the other hand, from the viewpoint of patterning properties, the content of the binder resin is preferably 60% by mass or less, and more preferably 50% by mass or less, based on the solid content.

[0038] The coloring composition of the present invention contains a radical polymerizable compound, and the radical polymerizable compound contains dipentaerythritol hexa(meth)acrylate and pentaerythritol tri(meth)acrylate. The total content of dipentaerythritol hexa(meth)acrylate and pentaerythritol tri(meth)acrylate in the radical polymerizable compound is preferably 70% by mass or more from the viewpoints of preventing color mixing, suppressing color transfer, suppressing pin unevenness, and solubility and processability during overcoating processing. The radical polymerizable compound referred to here refers to a compound that reacts by radical polymerization and refers to a compound having a weight average molecular weight of 1,000 or less. The radical polymerizable compound is preferably a compound having an unsaturated hydrocarbon group. Examples of the unsaturated hydrocarbon group include a (meth)acryloyl group, a vinyl group, and a maleimide group. Two or more of these may be included. The coloring composition of the present invention may also contain a radical polymerizable compound other than dipentaerythritol hexa(meth)acrylate and pentaerythritol tri(meth)acrylate.

[0039] Examples of radical polymerizable compounds other than dipentaerythritol hexa(meth)acrylate and pentaerythritol tri(meth)acrylate include ethylene oxide modified compounds or propylene oxide modified compounds such as dipentaerythritol penta(meth)acrylate, tetratrimethylolpropane tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, and penta(meth)acryloyloxydipentaerythritol monosuccinic acid ester, styrene derivatives, polyfunctional maleimide compounds, poly(meth)acrylate carbamates, adipic acid 1,6-hexanediol (meth)acrylic acid ester, and phthalic anhydride. Examples of suitable (meth)acrylates include propylene oxide (meth)acrylate, diethylene glycol trimellitic (meth)acrylate, rosin-modified epoxy di(meth)acrylate, alkyd-modified (meth)acrylate and other oligomers, tripropylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate and other bifunctional (meth)acrylates, trimethylolpropane tri(meth)acrylate, triacrylformal, bisphenoxyethanol fluorene diacrylate, dicyclopentadienyl diacrylate, and alkyl-modified, alkyl ether-modified and alkyl ester-modified products thereof.

[0040] The coloring composition of the present invention contains dipentaerythritol hexa(meth)acrylate and pentaerythritol tri(meth)acrylate, and the ratio of the weight (A) of the dipentaerythritol hexa(meth)acrylate to the weight (B) of the pentaerythritol tri(meth)acrylate is 0.16

[0041] The content of the radical polymerizable compound in the coloring composition of the present invention is preferably 40% by mass or more in the solid content from the viewpoint of patterning property. On the other hand, from the viewpoint of suppressing unevenness in film thickness during film formation and suppressing deformation of the pattern due to flow during baking, the content of the radical polymerizable compound is preferably 90% by mass or less in the solid content, more preferably 70% by mass or less, and even more preferably 60% by mass or less. In addition, from the viewpoint of patterning property, the content of the radical polymerizable compound having three or more (meth)acryloyl groups and carboxyl groups is preferably 50% by mass or more in the radical polymerizable compound, and even more preferably 60% by mass or more.

[0042] ​The coloring composition of the present invention contains a photopolymerization initiator. By containing a photopolymerization initiator, the sensitivity during patterning can be improved. Here, the photopolymerization initiator refers to a compound that decomposes and / or reacts with light (including ultraviolet light or electron beam) to generate radicals. Examples of the photopolymerization initiator include oxime ester compounds, benzophenone compounds, acetophenone compounds, oxanthone compounds, anthraquinone compounds, imidazole compounds, benzothiazole compounds, benzoxazole compounds, carbazole compounds, triazine compounds, phosphorus compounds, and titanocene compounds.

[0043] More specifically, examples of the oxime ester compounds include 1,2-octanedione, 1-[4-(phenylthio)phenyl]-, 2-(O-benzoyloxime), ethanone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-, 1-(O-acetyloxime), ethanone, 1-[9-ethyl-6-(2-methyl-4-tetrahydrofuranylmethoxybenzoyl)-9H-carbazol-3-yl]-, 1-(O-acetyloxime), ethanone, Examples of the benzophenone compounds include 1-[9-ethyl-6-{2-methyl-4-(2,2-dimethyl-1,3-dioxolanyl)methoxybenzoyl}-9H-carbazol-3-yl]-, 1-(O-acetyloxime), 1,2-octanedione, 1-[4-(phenylthio)-2-(O-benzoyloxime)], "ADEKA ACURE" (registered trademark) N-1919, NCI-930 (manufactured by ADEKA Corporation), "IRGACURE" (registered trademark) OXE01, OXE02 (manufactured by BASF Japan Co., Ltd.), etc. Examples of the benzophenone compounds include benzophenone, N,N'-tetraethyl-4,4'-diaminobenzophenone, 4-methoxy-4'-dimethylaminobenzophenone, etc. Examples of acetophenone compounds include 2,2-diethoxyacetophenone, benzoin, benzoin methyl ether, benzoin isobutyl ether, benzyl dimethyl ketal, α-hydroxyisobutylphenone, 1-hydroxycyclohexyl phenyl ketone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-1-propane, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone, 2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butanone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one, and "IRGACURE" (registered trademark) 369, 379, and 907 (manufactured by BASF Japan Ltd.).Examples of anthraquinone compounds include t-butylanthraquinone, 1-chloroanthraquinone, 2,3-dichloroanthraquinone, 3-chloro-2-methylanthraquinone, 2-ethylanthraquinone, 1,4-naphthoquinone, 9,10-phenanthraquinone, 1,2-benzoanthraquinone, 1,4-dimethylanthraquinone, and 2-phenylanthraquinone. Examples of imidazole compounds include 2-(o-chlorophenyl)-4,5-diphenylimidazole dimer. Examples of benzothiazole compounds include 2-mercaptobenzothiazole. Examples of benzoxazole compounds include 2-mercaptobenzoxazole. Examples of triazine compounds include 4-(p-methoxyphenyl)-2,6-di-(trichloromethyl)-s-triazine. Two or more of these may be contained, and it is more preferable to use a photosensitizer described later in combination from the viewpoint of suppressing color transfer and preventing color mixing.

[0044] The content of the photopolymerization initiator is preferably 1% by mass or more, more preferably 2% by mass or more, and even more preferably 5% by mass or more, based on the solid content of the coloring composition excluding the coloring material, from the viewpoints of sensitivity, patterning ability, processability, and heat resistance. On the other hand, the content of the photopolymerization initiator is preferably 30% by mass or less, more preferably 20% by mass or less, and even more preferably 15% by mass or less, based on the solid content of the coloring composition excluding the coloring material, from the viewpoints of sensitivity, patterning ability, processability, and heat resistance.

[0045] The colored composition of the present invention may further contain a dispersant, a chain transfer agent, a photosensitizer, an organic solvent, a polymerization inhibitor, an adhesion improver, a surfactant, an organic acid, an organic amino compound, a curing agent, and the like.

[0046] The coloring material contained in the coloring composition of the present invention can be identified by laser Raman spectroscopy (Ar+ laser (457.9 nm)) or mass spectrometry using a MALDI mass spectrometer or a time-of-flight secondary ion mass spectrometer.

[0047] The content of the coloring material in the coloring composition can be quantified by mass analysis using a MALDI mass spectrometer or a time-of-flight secondary ion mass spectrometer, and the ratio (mass%) of the coloring material to the solid content of the coloring composition can be calculated from the mass of the coloring material and the content of other components. When the blending ratio of the raw materials of the coloring composition is known, the ratio (mass%) of the coloring material to the solid content of the coloring composition can be calculated from the blending amount of the coloring material and the blending amount of other components.

[0048] The coloring composition of the present invention may contain a dispersant such as a pigment derivative together with the colorant. Examples of the dispersant include low molecular weight dispersants such as pigment intermediates and derivatives, and polymeric dispersants. Examples of the pigment derivative include alkylamine-modified pigment skeletons, carboxylic acid derivatives, and sulfonic acid derivatives, which contribute to appropriate wetting and stabilization of the pigment. Sulfonic acid derivatives of the pigment skeleton are preferred, as they have a significant effect on stabilizing fine pigments.

[0049] Examples of polymer dispersants include polyester, polyalkylamine, polyallylamine, polyimine, polyamide, polyurethane, polyacrylate, polyimide, polyamideimide, and copolymers thereof. Two or more of these may be contained. Among these polymer dispersants, those having an amine value of 5 to 200 mgKOH / g and an acid value of 1 to 100 mgKOH / g in terms of solid content are preferred. Among them, polymer dispersants having a basic group are preferred, and can improve the storage stability of the pigment dispersion and the coloring composition. Examples of commercially available polymer dispersants having a basic group include "Solsperse" (registered trademark) (manufactured by Lubrizol Japan Co., Ltd.), "Efka" (registered trademark) (manufactured by BASF), "Ajisper" (registered trademark) (manufactured by Ajinomoto Fine-Techno Co., Ltd.), and "BYK" (registered trademark) (manufactured by BYK Japan Co., Ltd.). Two or more of these may be contained. Among these, "Solsperse" (registered trademark) 24000 (manufactured by Lubrizol Japan Co., Ltd.), "EFKA" (registered trademark) 4300, 4330 (manufactured by BASF), 4340 (manufactured by BASF), "Ajisper" (registered trademark) PB821, PB822 (manufactured by Ajinomoto Fine-Techno Co., Ltd.), and "BYK" (registered trademark) 161 to 163, 2000, 2001, 6919, 21116 (manufactured by BYK Japan KK) are preferred.

[0050] When the coloring composition of the present invention contains a polymer dispersant, the total content of the polymer dispersant and the binder resin is preferably 10% by mass or more, more preferably 20% by mass or more, and even more preferably 30% by mass or more in the solid content from the viewpoint of suppressing unevenness in the film thickness during film formation. On the other hand, from the viewpoint of patterning property, the total content of the polymer dispersant and the binder resin is preferably 60% by mass or less, more preferably 50% by mass or less in the solid content excluding the coloring material of the coloring composition.

[0051] The coloring composition of the present invention may contain a chain transfer agent together with the photopolymerization initiator, and the sensitivity can be further improved. Examples of the chain transfer agent include thioglycolic acid, thiomalic acid, thiosalicylic acid, 2-mercaptopropionic acid, 3-mercaptopropionic acid, 3-mercaptobutyric acid, N-(2-mercaptopropionyl)glycine, 2-mercaptonicotinic acid, 3-[N-(2-mercaptoethyl)carbamoyl]propionic acid, 3-[N-(2-mercaptoethyl)amino]propionic acid, N-(3-mercaptopropionyl)alanine, 2-mercaptoethanesulfonic acid, 3-mercaptopropanesulfonic acid, 4-mercaptobutanesulfonic acid, dodecyl(4-methylthio)phenyl ether, 2-mercaptoethanol, 3-mercapto-1,2 -propanediol, 1-mercapto-2-propanol, 3-mercapto-2-butanol, mercaptophenol, 2-mercaptoethylamine, 2-mercaptoimidazole, 2-mercapto-3-pyridinol, 2-mercaptobenzothiazole, mercaptoacetic acid, trimethylolpropane tris(3-mercaptopropionate), 1,3,5-tris(3-mercaptobutyloxyethyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione), pentaerythritol tetrakis(3-mercaptopropionate), 1,4-bis(3-mercaptobutyryloxy)butane, "Kalends" (registered trademark) MT Examples of the mercapto compounds include PE-1 (manufactured by Showa Denko K.K.), Karenz (registered trademark) MT NR-1 (manufactured by Showa Denko K.K.), Karenz (registered trademark) MT BD-1 (manufactured by Showa Denko K.K.), etc., disulfide compounds obtained by oxidizing the mercapto compounds, and iodized alkyl compounds such as iodoacetic acid, iodopropionic acid, 2-iodoethanol, 2-iodoethanesulfonic acid, and 3-iodopropanesulfonic acid. Two or more of these may be contained.

[0052] From the viewpoint of preventing color mixing, the coloring composition of the present invention preferably further contains a photosensitizer. Examples of the photosensitizer include thioxanthone-based sensitizers, aromatic or aliphatic tertiary amines, and the like. Examples of the thioxanthone-based sensitizer include thioxanthone, 2-chlorothioxanthone, 2,4-diethylthioxanthen-9-one, "KAYACURE" (registered trademark) DETX-S (manufactured by Nippon Kayaku Co., Ltd.), and the like. Two or more of these may be contained. From the viewpoints of suppressing color migration and preventing color mixing of the coloring composition of the present invention, thioxanthone-based sensitizers are preferred. Further, from the viewpoints of suppressing color migration and preventing color mixing, it is preferable that the ratio of the weight (K) of the photosensitizer to the weight (L) of the photopolymerization initiator is 0.3 < K / L < 0.6.

[0053] The coloring composition of the present invention contains an organic solvent. Examples of the organic solvent include diethylene glycol monobutyl ether acetate, benzyl acetate, ethyl benzoate, methyl benzoate, diethyl malonate, 2-ethylhexyl acetate, 2-butoxyethyl acetate, ethylene glycol monobutyl ether acetate, diethyl oxalate, ethyl acetoacetate, cyclohexyl acetate, 3-methoxy-butyl acetate, methyl acetoacetate, ethyl 3-ethoxypropionate, 2-ethylbutyl acetate, isopentyl propionate, propylene glycol monomethyl ether propionate, pentyl acetate, propylene glycol monomethyl ether acetate, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, propylene glycol monoethyl ether, diethylene glycol monomethyl ether, monoethyl ether, methyl carbitol, ethyl carbitol, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol tertiary butyl ether, dipropylene glycol monomethyl ether, ethyl acetate, butyl acetate, isopentyl acetate, butanol, 3-methyl-2-butanol, 3-methyl-3-methoxybutanol, cyclopentanone, cyclohexanone, xylene, ethylbenzene, solvent naphtha, and the like. Two or more of these may be contained.

[0054] In the coloring composition of the present invention, the ratio of the weight (P) of the components excluding the coloring agent, radical polymerizable compound, photopolymerization initiator, and organic solvent contained in the coloring composition to the weight (R) of the radical polymerizable compound is 0.5 < P / R < 1.2. When P / R is 1.2 or more, suppression of color migration, solubility during overcoating, and processability become insufficient. Preferably, P / R < 1.1, more preferably P / R < 0.9. Also, when P / R is 0.5 or less, film-forming properties and pinhole suppression become insufficient. Preferably, P / R > 0.4, more preferably P / R > 0.5, and particularly preferably P / R > 0.65.

[0055] In the case of a preferred embodiment in which the coloring composition of the present invention contains a photosensitizer, it is more preferable that the ratio of the weight (P) of the components excluding the coloring agent, radical polymerizable compound, photopolymerization initiator, organic solvent, and photosensitizer contained in the coloring composition to the weight (R) of the radical polymerizable compound is 0.5 < P / R < 1.2. By setting P / R to 0.5 < P / R < 1.2, a preferable composition can be obtained from the viewpoints of suppressing color migration of the dye, film-forming properties, pinhole suppression, solubility during overcoating, and processability. From the viewpoint of suppressing color migration, the ratio P / R of the weight (P) of the components excluding the coloring agent, radical polymerizable compound, photopolymerization initiator, organic solvent, and photosensitizer contained in the coloring composition to the weight (R) of the radical polymerizable compound is more preferably P / R < 1.1, and even more preferably P / R < 0.9. Also, from the viewpoints of solubility and processability during overcoating, the ratio P / R of the weight (P) of the components excluding the coloring agent, radical polymerizable compound, photopolymerization initiator, organic solvent, and photosensitizer contained in the coloring composition to the weight (R) of the radical polymerizable compound is more preferably P / R < 1.1, and even more preferably P / R < 0.9. Also, from the viewpoints of film-forming properties and pinhole suppression, more preferably P / R > 0.65.

[0056] The coloring composition of the present invention may further contain a polymerization inhibitor, which can improve stability. Polymerization inhibitors generally have the effect of inhibiting or terminating polymerization caused by radicals generated by heat, light, radical initiators, etc., and are generally used to prevent gelation of thermosetting resins and to terminate polymerization during polymer production. Examples of polymerization inhibitors include hydroquinone, tert-butylhydroquinone, 2,5-bis(1,1,3,3-tetramethylbutyl)hydroquinone, 2,5-bis(1,1-dimethylbutyl)hydroquinone, catechol, and tert-butylcatechol. Two or more of these may be contained. From the viewpoint of the balance between stability and photosensitive properties, the content of the polymerization inhibitor is preferably 0.0001% by mass or more in the solid content, and more preferably 0.005% by mass or more. Also, from the viewpoint of the balance between stability and photosensitive properties, the content of the polymerization inhibitor is preferably 1% by mass or less in the solid content, and more preferably 0.5% by mass or less.

[0057] The coloring composition of the present invention may further contain an adhesion improver, and the adhesion of the coating film of the coloring composition to the substrate can be improved. Examples of the adhesion improver include silane coupling agents such as vinyltrimethoxysilane, vinyltriethoxysilane, vinyltris(2-methoxyethoxy)silane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-chloropropylmethyldimethoxysilane, 3-chloropropyltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane, and 3-mercaptopropyltrimethoxysilane. Two or more of these may be contained.

[0058] The coloring composition of the present invention may further contain a surfactant, which can improve the coatability of the coloring composition and the uniformity of the coating film surface. Examples of the surfactant include anionic surfactants such as ammonium lauryl sulfate and triethanolamine polyoxyethylene alkyl ether sulfate, cationic surfactants such as stearylamine acetate and lauryltrimethylammonium chloride, amphoteric surfactants such as lauryldimethylamine oxide and lauryl carboxymethyl hydroxyethyl imidazolium betaine, nonionic surfactants such as polyoxyethylene lauryl ether, polyoxyethylene stearyl ether, and sorbitan monostearate, fluorine-based surfactants, and silicone-based surfactants. Two or more of these may be contained. From the viewpoint of in-plane uniformity of the coating film, the content of the surfactant is preferably 0.001 to 10% by mass in the coloring composition.

[0059] In the coloring composition of the present invention, it is preferable from the viewpoints of color bleeding suppression, solubility during overcoating, and processability that the molar number M of double bonds contained per gram T of the solid content excluding the colorant satisfies 160 < T / M < 220. Here, the solid content refers to all components excluding the organic solvent among the components contained in the coloring composition. From the viewpoints of color bleeding suppression, solubility during overcoating, and processability, the ratio T / M of the molar number M of double bonds contained per gram T of the solid content excluding the colorant is preferably T / M < 220, more preferably T / M < 200. Also, from the viewpoint of pinhole suppression, the ratio T / M of the molar number M of double bonds contained per gram T of the solid content excluding the colorant is preferably T / M > 160, more preferably T / M > 170.

[0060] Next, the color filter substrate of the present invention will be described. The color filter substrate of the present invention has pixels made of the coloring composition of the present invention on a substrate. Further, it may have a black matrix, a photo spacer, an overcoat layer, an alignment film, a polarizing plate, a retardation plate, an antireflection film, a transparent electrode, a diffusion plate, etc.

[0061] Examples of the substrate include inorganic glass plates such as soda glass, non-alkali glass, borosilicate glass, quartz glass, aluminoborosilicate glass, aluminosilicate glass, alkali aluminosilicate glass, and soda lime glass with a silica-coated surface, silicon wafers, and organic plastic films and sheets. Two or more of these may be laminated. In addition, when the display device having the color filter substrate of the present invention is a reflective display device or a display device having a light-emitting element such as a silicon OLED, the substrate may be opaque.

[0062] The organic plastic film or sheet may be a self-supporting film, or may be a film formed by coating on a substrate such as a glass substrate. In the case of such a coating film, the adhesion between the substrate and the film can be appropriately adjusted by a laser or the like to peel off the film. Examples of organic plastic materials include polyesters such as polypropylene, polyethylene, polystyrene, and polyethylene terephthalate (PET), fluorine-containing polymers such as polyphenylene sulfide (PPS), polyimide, polyamide, polyamideimide, polyethersulfone, and polytetrafluoroethylene (PTFE), polyetheretherketone, polyphenylene ether, polyarylate, and polysulfone. Even when baked at 100° C. or less, the colored composition of the present invention is unlikely to peel off during overcoating processing, and furthermore, color mixing of the pattern can be suppressed. Therefore, pixels can be formed even if a film that is likely to be deformed by heat is used as a substrate, and the color filter substrate can be suitably used for the manufacture of a film-like color filter substrate in which each colored pixel is formed on a film.

[0063] From the viewpoint of the strength of the substrate, the substrate is preferably a film having a thickness of 5 μm or more, more preferably 10 μm or more, whereas from the viewpoint of flexibility, the substrate is preferably a film having a thickness of 100 μm or less.

[0064] Examples of the pixels include colored pixels of red, blue, etc., and transparent pixels. Examples of materials constituting the pixels include the colored composition of the present invention, and colored photosensitive compositions containing a binder resin such as an acrylic resin or a polyimide resin and a radical polymerizable compound. From the viewpoint of improving color purity, the film thickness of the pixel is preferably 0.5 μm or more, more preferably 1.0 μm or more, and even more preferably 1.4 μm or more. On the other hand, from the viewpoint of improving the flatness, pattern processability, and reliability of the color filter substrate, the film thickness is preferably 3.0 μm or less, and more preferably 2.8 μm or less.

[0065] The black matrix prevents the contrast and color purity from decreasing due to light leakage between pixels, and is preferably disposed between pixels or in the frame. Examples of materials constituting the black matrix include a photosensitive composition containing a binder resin such as an acrylic resin or a polyimide resin and a radical polymerizable compound, and a non-photosensitive resin composition colored black. From the viewpoint of light shielding, the film thickness of the black matrix is ​​preferably 0.5 μm or more, more preferably 1.0 μm or more. On the other hand, from the viewpoint of processability, it is preferably 2.0 μm or less, more preferably 1.5 μm or less.

[0066] The photospacer provides a certain gap between the opposing substrates, and since a liquid crystal compound or the like can be filled in the gap, the step of arranging the spacer can be omitted during the manufacture of the liquid crystal display device. It is preferable that the photospacer is fixed to a specific location of the color filter substrate so as to be in contact with the opposing substrate when the liquid crystal display device is manufactured. Examples of materials constituting the photospacer include a photosensitive composition containing a binder resin such as an acrylic resin or a polyimide resin and a radical polymerizable compound. Examples of the shape of the photospacer include a cylindrical shape, a prismatic shape, a truncated cone shape, and a truncated pyramid shape. The diameter of the photospacer is not particularly specified, but is preferably 2 to 20 μm, more preferably 3 to 10 μm. The height of the photospacer is preferably 1 to 10 μm.

[0067] The overcoat layer suppresses the transmission of impurities from the pixels of the color filter substrate and flattens the steps caused by the pixels of the color filter substrate. Examples of materials constituting the overcoat layer include epoxy resin, acrylic epoxy resin, acrylic resin, siloxane resin, polyimide resin, and photosensitive or non-photosensitive materials commercially available as flattening materials. From the viewpoint of processability, the film thickness of the overcoat layer is preferably 0.5 μm or more, and more preferably 1.0 μm or more. On the other hand, from the viewpoint of flatness of the color filter substrate, the film thickness is preferably 5.0 μm or less, and more preferably 3.0 μm or less.

[0068] Examples of materials constituting the transparent electrodes include metals such as aluminum, chromium, tantalum, titanium, neodymium, and molybdenum, indium-tin-oxide (ITO), and indium-zinc-oxide (InZnO).

[0069] As a method for producing a color filter substrate, for example, a method for forming a pattern of pixels made of a resin composition on a substrate can be mentioned. The production method will be described below using a color filter substrate having pixels made of the coloring composition of the present invention as an example. The coloring composition of the present invention is applied onto a substrate, patterned by selective exposure and development using a photomask, and baked to form pixels, thereby obtaining a color filter substrate.

[0070] Examples of the method for applying the coloring composition of the present invention onto a substrate include a spin coater, a bar coater, a blade coater, a roll coater, a die coater, an inkjet printing method, a screen printing method, a method for immersing a substrate in a coloring composition, and a method for spraying a coloring composition onto a substrate. Subsequently, the substrate onto which the coloring composition has been applied is dried to form a coating film of the coloring composition on the substrate. Examples of the drying method include air drying, heat drying, and vacuum drying. Two or more of these may be combined, and for example, it is preferable to perform heat drying after performing reduced pressure drying. The temperature of the heat drying is preferably 80 to 130°C, and the heat drying device is preferably a hot air oven or a hot plate. In the case of a color filter substrate having a black matrix, it is preferable to form a coating film of the coloring composition on a substrate on which a black matrix has been formed in advance.

[0071] Next, a photomask is placed on the coating film of the colored composition, and selective exposure is performed. Examples of the exposure machine include a proximity exposure machine, a mirror projection exposure machine, a lens scan exposure machine, a stepper, etc. From the viewpoint of accuracy, the lens scan exposure machine is preferred. Examples of the light source used for exposure include an ultra-high pressure mercury lamp, a chemical lamp, a high pressure mercury lamp, etc.

[0072] Thereafter, the unexposed portion is removed by development with an alkaline developer to form a coating film pattern. Examples of the alkaline substance used in the alkaline developer include inorganic alkalis such as sodium hydroxide, potassium hydroxide, sodium carbonate, potassium carbonate, sodium silicate, sodium metasilicate, and aqueous ammonia, primary amines such as ethylamine and n-propylamine, secondary amines such as diethylamine and di-n-propylamine, tertiary amines such as triethylamine and methyldiethylamine, and organic alkalis such as tetramethylammonium hydroxide. Examples of the alkaline developer include 0.02 to 1 mass % potassium hydroxide or tetramethylammonium hydroxide. Examples of the development method include a method in which the coating film after exposure is immersed in an alkaline developer for 20 to 300 seconds.

[0073] Thereafter, the obtained coating film pattern is heat-treated to obtain a color filter substrate having a pixel pattern. The heat treatment may be performed in air, in a nitrogen atmosphere, or in a vacuum. The heating temperature is preferably 80 to 250°C. The heating time is preferably 5 minutes to 5 hours. As the heat treatment device, a hot air oven or a hot plate is preferable. The heat treatment may be performed continuously or stepwise. When the coloring composition of the present invention is used, even if it is baked at 100°C or less, the pattern is less likely to peel off during overcoating processing, and further, color mixing of the pattern can be suppressed. Therefore, it can be suitably used for manufacturing a color filter substrate by (A) applying the coloring composition of the present invention onto a substrate, (B) forming a pattern by exposure and development, and (D) performing a heat treatment at 100°C or less. In particular, when the coloring composition of the present invention is used, a color filter substrate can be produced by a heat treatment process at 100°C or less, so that a color filter substrate can be produced using a film that is easily denatured or deteriorated by heat, or a substrate including a device element such as an organic EL element that is easily denatured or deteriorated by heat.

[0074] In addition, it is preferable to form a pattern by applying the colored composition of the present invention onto a substrate, exposing and developing the pattern, and then exposing the pattern before performing heat treatment to form a pattern. By exposing the pattern before heat treatment, crosslinking can be further enhanced.

[0075] The pixels of 3 to 6 colors of the color filter substrate are sequentially formed by the above method. The order of forming the colors is not particularly limited, but when forming pixels containing dyes, it is preferable to form the pixels containing dyes after forming other pixels from the viewpoint of further suppressing color transfer of color materials.

[0076] The color filter substrate of the present invention can be used as a component of a display device such as a liquid crystal display, an organic EL display, or electronic paper. That is, the display device of the present invention has the color filter substrate of the present invention and a display element. Furthermore, the display device may have a light source such as an external light source, or various films such as a brightness enhancing film or a diffusion plate. The display device refers to a device that displays an image by allowing a part of the screen to be viewed. Examples of the display element include a liquid crystal element, an organic EL element, an inorganic EL element, a display element using MEMS, a display element using quantum dots, electronic ink, electronic liquid powder, and an electrophoretic element. Examples of the display device include a transmissive liquid crystal display, a semi-transmissive liquid crystal display, a reflective liquid crystal display, an organic EL display, an inorganic EL display, a quantum dot display, and electronic paper. Examples of the reflective display device include devices that display with outdoor light or indoor light, such as a wearable terminal, an electronic signboard, a digital signage, and an electronic shelf label. The coloring composition of the present invention can form colored pixels on a film, and therefore can be suitably used for electronic paper, curved displays, and flexible displays using a film-like color filter substrate. In addition, even if the colored composition of the present invention is baked at 100°C or less, pattern peeling during overcoating processing is unlikely to occur, and further color mixing of the pattern can be suppressed. Therefore, it can be formed on a substrate including an organic EL element that is likely to deteriorate due to heat, and therefore it can be suitably used for organic EL displays such as silicon OLED.

[0077] As an example of the manufacturing method of the display device of the present invention, a manufacturing method of a liquid crystal display device is described below. A color filter substrate and an array substrate are laminated facing each other via a liquid crystal alignment film and a spacer for maintaining a cell gap provided on the substrates. A TFT liquid crystal display device or a TFD liquid crystal display device can be manufactured by providing a thin film transistor (TFT) element or a thin film diode (TFD) element, a scanning line or a signal line, etc. on the array substrate. Next, liquid crystal is injected from an injection port provided in the sealing portion, and the injection port is sealed. Furthermore, a backlight is attached and an IC driver, etc. are mounted to complete the liquid crystal display device. As the backlight, a two-wavelength LED, a three-wavelength LED, a CCFL, etc. can be used, but a three-wavelength LED is preferable because it can expand the color reproduction range of the liquid crystal display device and keep power consumption low. EXAMPLES

[0078] The present invention will be described below with reference to examples, but the present invention is not limited to these examples. First, the evaluation methods in the examples and comparative examples will be described. Other components used in each example and comparative example are as follows.

[0079] Radical polymerizable compound solution D1: Dipentaerythritol hexaacrylate diluted to 50% by mass in propylene glycol monomethyl ether acetate solution D2: A propylene glycol monomethyl ether acetate solution containing pentaerythritol triacrylate diluted to 50% by mass Photoinitiator E1: "ADEKA Arcles" (registered trademark) NCI831 (manufactured by ADEKA Corporation) E2: "Irgacure" (registered trademark) 379 (manufactured by BASF Japan Ltd.) Photosensitizers F1: 2,4-Diethylthioxanthone Organic solvents G1: Propylene glycol monomethyl ether acetate <Peeling evaluation> The colored compositions obtained in Examples 1 to 8 and Comparative Examples 1 to 5 described below were applied onto a glass substrate and dried at 90°C for 10 minutes. Thereafter, the substrate was exposed to 40 mJ of i-line through a photomask having a 20 μm line and space pattern. Next, the substrate was shower-developed with a 0.3 mass% tetramethylammonium hydroxide aqueous solution at 23°C for 50 seconds, and then washed with pure water. The substrate was baked at 100°C for 30 minutes to obtain a substrate with a film having a thickness of 2.3 μm.

[0080] The colored composition (J1) obtained in Production Example 5 described later was applied to the obtained substrate with the film to a thickness of 2.3 μm, and dried for 10 minutes at 90° C. Shower development was performed for 90 seconds using a 0.3 mass% aqueous solution of tetramethylammonium hydroxide at 23° C. The presence or absence of a pattern on the substrate was confirmed using a microscope, and evaluated according to the following evaluation criteria. A: No pattern peeling B: Pattern peeling <Color mixing evaluation> The colored compositions obtained in Examples 1 to 8 and Comparative Examples 1 to 5 described below were applied onto a glass substrate and dried at 90° C. for 10 minutes. Thereafter, the substrate was irradiated with i-rays at 40 mJ / cm through a photomask having a 20 μm line and space pattern. 2 The substrate was exposed to light at 400 nm. The substrate was then shower-developed with a 0.3% by mass aqueous solution of tetramethylammonium hydroxide at 23° C. for 50 seconds, and then washed with pure water. The substrate was baked at 100° C. for 30 minutes to obtain a substrate with a coating having a thickness of 2.3 μm. The transmittance T0 of the obtained coating at 650 nm was measured using a microspectrophotometer LCF-100MA manufactured by Otsuka Electronics Co., Ltd.

[0081] Next, the colored composition (J1) obtained by Production Example 5 described later was applied onto the obtained substrate with the film under the condition that the film thickness after drying at 90° C. for 10 minutes was 2.3 μm. Then, after drying at 90° C. for 10 minutes, shower development was performed with a 0.3 mass% tetramethylammonium hydroxide aqueous solution at 23° C. for 90 seconds to obtain a substrate with the film. The obtained film was measured for transmittance T1 at 650 nm using a microspectrophotometer LCF-100MA manufactured by Otsuka Electronics Co., Ltd., and color mixing was evaluated by T1 / T0. The closer the value of T1 / T0 is to 1, the less likely color mixing occurs, and this is preferable. In the color mixing evaluation, when no pattern remains, it is marked as "-".

[0082] <Pin Mura Evaluation> The composition for black matrix (J2) obtained in Production Example 6 described below was spin-coated on a glass substrate and dried at 120° C. for 120 seconds. The resulting coating film was exposed to i-rays at 200 mJ / cm 2 After exposure to light at 400 K, the substrate was immersed in a 2.0% by mass aqueous solution of sodium hydroxide for 2 minutes, washed with pure water, and baked in an oven at 230° C. for 30 minutes to obtain a black matrix substrate on which a 1.5 μm film was formed.

[0083] The colored compositions obtained in Examples 1 to 8 and Comparative Examples 1 to 5 described below were applied onto the obtained black matrix substrate, and then the substrate was placed on a cylindrical base (made of polyethylene) with a diameter of 1.5 cm and a height of 1 cm and dried under reduced pressure until the pressure reached 40 Pa. The substrate was then dried on a hot plate at 100° C. for 3 minutes. The obtained substrate was visually inspected under a Na lamp to check for the presence or absence of unevenness resulting from the cylindrical base, and evaluated according to the following evaluation criteria. A: No unevenness due to the base B: There are uneven spots due to the base. <Color transfer resistance> The photosensitive compositions for color filters obtained in Examples 1 to 8 and Comparative Examples 1 to 5 described below were spin-coated on a glass substrate and dried for 10 minutes at 90° C. The resulting coating film was exposed to i-rays at 40 mJ / cm 2After exposure to 1000 Hz, the substrate was shower-developed with a 0.3% by mass aqueous solution of tetramethylammonium hydroxide at 23° C. for 50 seconds, and then washed with pure water. The substrate was baked at 230° C. for 30 minutes to obtain a substrate on which a film having a thickness of 2.3 μm was formed. The colored composition (J3) obtained in Production Example 7 described later was spin-coated on the obtained substrate, and dried at 90° C. for 10 minutes. The obtained coating film was irradiated with 200 mJ / cm of i-line through a photomask having a circular pattern with a diameter of 30 μm. 2 After exposure to 100° C., the substrate was shower-developed for 50 seconds with a 0.3% by mass aqueous solution of tetramethylammonium hydroxide at 23° C., and washed with pure water to obtain a substrate with a film having a circular hole with a thickness of 2 μm and a diameter of 30 μm. The brightness Y0 of the center of the circular hole was measured using a microspectrometer LCF-100MA manufactured by Otsuka Electronics Co., Ltd. Next, the substrate with the film was baked at 230° C. for 30 minutes, and the brightness Y1 of the center of the circular hole was measured, and Y1 / Y0 was calculated to evaluate the color transfer resistance, which is an index of the difficulty of the phenomenon in which a coloring material in a pixel formed later penetrates into a pixel formed earlier. The closer the value of Y1 / Y0 is to 1, the less likely color transfer occurs, and this is preferable.

[0084] <Solubility evaluation> The colored compositions obtained in Examples 1 to 8 and Comparative Examples 1 to 5 described below were applied onto a glass substrate and dried at 90°C for 10 minutes. Thereafter, the substrate was exposed to 40 mJ of i-rays through a photomask, and then shower-developed with a 0.3% by mass aqueous solution of tetramethylammonium hydroxide at 23°C for 50 seconds, followed by washing with pure water. Next, the substrate was baked at 100°C for 30 minutes to obtain a substrate with a film having a thickness of 2.3 μm.

[0085] The colored composition (J1) obtained by Production Example 5 described later was applied to the obtained substrate with the film to a thickness of 2.3 μm, and dried for 10 minutes at 90° C. Shower development was performed with a 0.3 mass% tetramethylammonium hydroxide aqueous solution at 23° C., and the time until the coloring derived from the colored composition (J1) disappeared was confirmed, and the result was evaluated according to the following evaluation criteria. A: The time it takes for the coloring derived from the coloring composition (J1) to disappear is within 30 seconds B: The time it takes for the coloring derived from the coloring composition (J1) to disappear is 30 to 60 seconds. C: The time it takes for the coloring derived from the coloring composition (J1) to disappear is 60 seconds or more. Production Example 1 (Preparation of Dispersion (A1)) In a 500 mL three-neck flask under a nitrogen atmosphere, 176.3 g of anhydrous tert-amyl alcohol (2.0 mol) and 114.7 g of sodium tert-amyl alkoxide (1.1 mol) were placed, and the internal temperature was raised to 100° C. with stirring to react them, thereby preparing an alcoholate solution.

[0086] Into another 500 mL three-neck flask, 84.9 g of diisopropyl succinate (0.4 mol) and 145.6 g of 4-bromobenzonitrile (0.8 mol) were charged, and the internal temperature was raised to 85° C. with stirring to dissolve, thereby preparing a mixed solution.

[0087] The internal temperature of the three-neck flask containing the alcoholate solution was adjusted to 100° C., and the mixed solution was added dropwise over 3 hours while stirring. After the dropwise addition was completed, the mixture was heated and stirred at an internal temperature of 90° C. for 12 hours to obtain a suspension.

[0088] Further, 640 g of methanol (20.0 mol), 720 g of water (40.0 mol) and 300 g of acetic acid (10.0 mol) were charged into another 500 mL three-neck flask, and the mixture was stirred while cooling the internal temperature to -10°C to obtain a mixture.

[0089] The above suspension was added dropwise over 3 hours while stirring at high speed and keeping the internal temperature of the three-neck flask containing the above mixture below -5°C. After the dropwise addition, the mixture was stirred for another 7 hours, and then the reaction solution was washed and filtered until the filtrate was no longer colored and salt precipitation disappeared. The collected filtrate was dried at 80°C for 24 hours, and the resulting solid was pulverized to obtain 112 g of diketopyrrolopyrrole pigment having a bromine group (formula (1)). Further diketopyrrolopyrrole pigment having a bromine group was synthesized by the same method, and 150 g of diketopyrrolopyrrole pigment having a bromine group was prepared.

[0090] [ka]

[0091] 150 g of the obtained diketopyrrolopyrrole pigment having a bromine group, 66.6 g of "BYK" (registered trademark) LPN6919 (manufactured by BYK Japan Co., Ltd., polymer dispersant solution (60 mass% propylene glycol monomethyl ether solution)), 88.9 g of "Cyclomer" (registered trademark) ACA250 (manufactured by Daicel Chemical Co., Ltd., 45 mass% dipropylene glycol monomethyl ether solution), and 694.5 g of propylene glycol monomethyl ether (PMA) were mixed to prepare a slurry. The beaker containing the slurry was connected to a dyno mill with a tube, and a dispersion treatment was performed for 8 hours at a peripheral speed of 14 m / s using zirconia beads with a diameter of 0.5 mm as a medium, to prepare a diketopyrrolopyrrole pigment dispersion (A1) having a bromine group.

[0092] Production Example 2 (Preparation of Dispersion (A2)) A CI Pigment Red 177 dispersion (A2) was prepared in the same manner as in Production Example 1, except that 150 g of CI Pigment Red 177 was used instead of the diketopyrrolopyrrole pigment having a bromine group.

[0093] Production Example 3 (Preparation of Dispersion (A3)) A CI Pigment Blue 15:6 dispersion (A3) was prepared in the same manner as in Production Example 1, except that 150 g of CI Pigment Blue 15:6 was used instead of the diketopyrrolopyrrole pigment having a bromine group.

[0094] Production Example 4 (Synthesis of binder resin solution (B1)) In a 500 mL three-neck flask, 33 g (0.3 mol) of methyl methacrylate, 33 g (0.3 mol) of styrene, 35 g (0.5 mol) of methacrylic acid, 3 g (0.02 mol) of 2,2'-azobis (2-methylbutyronitrile) and 150 g of propylene glycol monomethyl ether acetate (PGMEA) were charged, and the mixture was stirred at 90 ° C for 2 hours, and then the internal temperature was raised to 100 ° C. and stirred for another hour to obtain a reaction solution. 33 g (0.2 mol) of glycidyl methacrylate, 1.2 g (0.009 mol) of dimethylbenzylamine and 0.2 g (0.002 mol) of p-methoxyphenol were added to the obtained reaction solution, and the mixture was stirred at 90 ° C. for 4 hours, and then PGMEA was added to obtain a binder resin solution (B1) with a solid content concentration of 40 mass%. The acid value of the binder resin was measured in a 0.1 mol / L potassium hydroxide-ethanol solution using an automatic potentiometer AT-610 manufactured by Kyoto Electronics Manufacturing Co., Ltd., and was found to be 119 (mgKOH / g). The weight average molecular weight calculated in terms of polystyrene was calculated using a GPC device and was found to be 22,000.

[0095] Production Example 5 (Preparation of Colored Composition (J1)) Into a 50 mL plastic bottle, 4.71 g of the dispersion (A3) obtained in Production Example 3, 3.05 g of the binder resin solution (B1) obtained in Production Example 4, 2.87 g of the radical polymerizable compound solution (D1), 0.57 g of "Irgacure" (registered trademark) 907 (manufactured by BASF Japan Ltd.), and 18.80 g of the organic solvent propylene glycol monomethyl ether acetate (G1) were added and stirred for 3 hours to prepare a colored composition (J1).

[0096] Production Example 6 (Preparation of Black Matrix Composition (J2)) 30 g of carbon powder (MA-8, manufactured by Mitsubishi Materials Corporation), 20 g of acrylic copolymer solution ("Cyclomer" (registered trademark) P ACA-250, manufactured by Daicel Chemical Industries, Ltd.), and 37 g of cyclohexanone were mixed and dispersed for 1 hour using a homogenizer. Then, 10 g of dipentaerythritol hexaacrylate and 3 g of a photopolymerization initiator "IRGACURE" (registered trademark) 369 (manufactured by Chiba Specialty Chemicals Corp.) were mixed therein to obtain a composition for black matrix (J2).

[0097] Production Example 7 (Preparation of Colored Composition (J3)) Into a three-neck flask, 15 g of Acid Red 289, 150 g of chloroform, and 8.9 g of N,N-dimethylformamide were added. The mixture was then cooled to below 20°C, and 10.9 g of thionyl chloride was added dropwise. After the dropwise addition, the mixture was heated to 50°C and stirred for 5 hours, then cooled to 20°C, and a mixture of 12.5 g of 2-ethylhexylamine and 22.1 g of triethylamine was added, and the mixture was stirred at 20°C for 5 hours to obtain a reaction mixture. The solvent was removed from the reaction mixture using a rotary evaporator, and the mixture was purified to obtain 10 g of a xanthene dye.

[0098] A slurry was prepared by mixing 10 g of the obtained xanthene dye, 90 g of PB15:6, 67 g of "BYK" (registered trademark) 6919, 67 g of "Cyclomer" ACA250, and 766 g of PMA. The beaker containing the slurry was connected to a Dyno Mill via a tube, and a dispersion treatment was carried out for 8 hours at a peripheral speed of 10 m / s using zirconia beads with a diameter of 0.3 mm as a medium, to prepare a dispersion liquid (A4) containing the dye.

[0099] In a 200 mL plastic bottle, 19.8 g of the obtained dispersion (A4), 23.16 g of the binder resin solution (B1) obtained in Production Example 4, 23.50 g of "Kayarad" (registered trademark) DPHA (manufactured by Nippon Kayaku Co., Ltd., multifunctional radical polymerizable compound), 0.31 g of "ADEKA ARCLES" (registered trademark) N-1919 (manufactured by ADEKA Corporation, oxime ester photopolymerization initiator), and 60.00 g of dipropylene glycol methyl ether acetate (DPMA) were added and stirred for 3 hours to prepare a colored composition (J3). Example 1 In a 50mL plastic bottle, 11.09g of the dispersion (A1) obtained by Production Example 1, 4.75g of the dispersion (A2) obtained by Production Example 2, 1.19g of the binder resin solution (B1) obtained by Production Example 4, 2.99g of the radical polymerizable compound solution (D1), 1.28g of the radical polymerizable compound solution (D2), 0.07g of the photopolymerization initiator (E1), 0.14g of the photopolymerization initiator (E2), 0.07g of the photosensitizer 2,4-diethylthioxanthone (F1), and 23.43g of the organic solvent propylene glycol monomethyl ether acetate (G1) were added and stirred for 3 hours to prepare a colored composition (H1). When the obtained colored composition was evaluated for peeling by the above method, no pattern peeling was observed. In addition, when the color mixing evaluation was performed by the above method, T1 / T0 was 0.94. Furthermore, when pin unevenness was evaluated by the above-mentioned method, unevenness due to the base was not confirmed. Furthermore, when color transfer was evaluated by the above-mentioned method, Y1 / Y0 was 0.99. Example 2 A colored composition (H2) was prepared in the same manner as in Example 1, except that the amount of radical polymerizable compound (D1) added was changed to 2.13 g, and the amount of radical polymerizable compound solution (D2) added was changed to 2.13 g. The obtained colored composition was used to perform a peeling evaluation by the above method, and no pattern peeling was observed. In addition, a color mixing evaluation was performed by the above method, and T1 / T0 was 0.96. In addition, a pin unevenness evaluation was performed by the above method, and no unevenness due to the base was observed. In addition, a color transfer evaluation was performed by the above method, and Y1 / Y0 was 0.99. Example 3 A colored composition (H3) was prepared in the same manner as in Example 1, except that the amount of radical polymerizable compound (D1) added was changed to 1.07 g, and the amount of radical polymerizable compound solution (D2) added was changed to 3.20 g. The obtained colored composition was used to perform a peeling evaluation by the above method, and no pattern peeling was observed. In addition, a color mixing evaluation was performed by the above method, and T1 / T0 was 0.98. In addition, a pin unevenness evaluation was performed by the above method, and no unevenness due to the base was observed. In addition, a color transfer evaluation was performed by the above method, and Y1 / Y0 was 0.99. Example 4 A colored composition (H4) was prepared in the same manner as in Example 1, except that the amount of radical polymerizable compound (D1) added was changed to 0.64 g, and the amount of radical polymerizable compound solution (D2) added was changed to 3.63 g. The obtained colored composition was used to perform a peeling evaluation by the above method, and no pattern peeling was observed. In addition, a color mixing evaluation was performed by the above method, and T1 / T0 was 0.99. In addition, a pin unevenness evaluation was performed by the above method, and no unevenness due to the base was observed. In addition, a color transfer evaluation was performed by the above method, and Y1 / Y0 was 0.99. Example 5 A colored composition (H5) was prepared in the same manner as in Example 1, except that the amount of binder resin solution (B1) obtained in Production Example 4 was changed to 0.71 g, the amount of radical polymerizable compound (D1) was changed to 3.26 g, and the amount of radical polymerizable compound solution (D2) was changed to 1.40 g. Using the obtained colored composition, peeling evaluation was performed by the above method, and no pattern peeling was observed. In addition, color mixing evaluation was performed by the above method, and T1 / T0 was 0.95. In addition, pin unevenness evaluation was performed by the above method, and no unevenness due to the base was observed. In addition, color transfer evaluation was performed by the above method, and Y1 / Y0 was 1.00. Example 6 A colored composition (H6) was prepared in the same manner as in Example 1, except that the amount of binder resin solution (B1) obtained in Production Example 4 was changed to 0.71 g, the amount of radical polymerizable compound (D1) was changed to 1.86 g, and the amount of radical polymerizable compound solution (D2) was changed to 2.79 g. Using the obtained colored composition, peeling evaluation was performed by the above method, and no pattern peeling was observed. In addition, color mixing evaluation was performed by the above method, and T1 / T0 was 0.98. In addition, pin unevenness evaluation was performed by the above method, and no unevenness due to the base was observed. In addition, color transfer evaluation was performed by the above method, and Y1 / Y0 was 1.00. Example 7 A colored composition (H7) was prepared in the same manner as in Example 1, except that the amount of binder resin solution (B1) obtained in Production Example 4 was changed to 1.68 g, the amount of radical polymerizable compound (D1) was changed to 2.71 g, and the amount of radical polymerizable compound solution (D2) was changed to 1.16 g. Using the obtained colored composition, peeling evaluation was performed by the above method, and no pattern peeling was observed. In addition, color mixing evaluation was performed by the above method, and T1 / T0 was 0.94. In addition, pin unevenness evaluation was performed by the above method, and no unevenness due to the base was observed. In addition, color transfer evaluation was performed by the above method, and Y1 / Y0 was 0.98. Example 8 A colored composition (H8) was prepared in the same manner as in Example 1, except that the amount of binder resin solution (B1) obtained in Production Example 4 was changed to 1.68 g, the amount of radical polymerizable compound (D1) was changed to 1.55 g, and the amount of radical polymerizable compound solution (D2) was changed to 2.33 g. Using the obtained colored composition, peeling evaluation was performed by the above method, and no pattern peeling was observed. In addition, color mixing evaluation was performed by the above method, and T1 / T0 was 0.98. In addition, pin unevenness evaluation was performed by the above method, and no unevenness due to the base was observed. In addition, color transfer evaluation was performed by the above method, and Y1 / Y0 was 0.98. Comparative Example 1 A colored composition (H9) was prepared in the same manner as in Example 1, except that the amount of radical polymerizable compound (D1) added was changed to 3.28 g, and the amount of radical polymerizable compound solution (D2) added was changed to 0.98 g. The obtained colored composition was used to perform peeling evaluation by the above method, and no pattern peeling was observed. In addition, when color mixing evaluation was performed by the above method, T1 / T0 was 0.71. In addition, when pin unevenness evaluation was performed by the above method, no unevenness due to the base was observed. In addition, when color transfer evaluation was performed by the above method, Y1 / Y0 was 0.99. Comparative Example 2 A colored composition (H10) was prepared in the same manner as in Example 1, except that the amount of radical polymerizable compound (D1) added was changed to 0.00 g, and the amount of radical polymerizable compound solution (D2) added was changed to 4.26 g. The obtained colored composition was used to perform a peeling evaluation by the above method, and pattern peeling was confirmed. In addition, when a color mixing evaluation was performed by the above method, no pattern remained. In addition, when a pin unevenness evaluation was performed by the above method, unevenness due to the base was not confirmed. In addition, when a color transfer evaluation was performed by the above method, Y1 / Y0 was 0.99. Comparative Example 3 A colored composition (H11) was prepared in the same manner as in Example 1, except that the amount of binder resin solution (B1) obtained in Production Example 4 was changed to 1.68 g, the amount of radical polymerizable compound (D1) was changed to 3.10 g, and the amount of radical polymerizable compound solution (D2) was changed to 0.78 g. Using the obtained colored composition, peeling evaluation was performed by the above method, and no pattern peeling was observed. In addition, color mixing evaluation was performed by the above method, and T1 / T0 was 0.63. In addition, pin unevenness evaluation was performed by the above method, and no unevenness due to the base was observed. In addition, color transfer evaluation was performed by the above method, and Y1 / Y0 was 0.98. Comparative Example 4 A colored composition (H12) was prepared in the same manner as in Example 1, except that the amount of binder resin solution (B1) obtained in Production Example 4 was changed to 0.03 g, the amount of radical polymerizable compound (D1) was changed to 3.64 g, and the amount of radical polymerizable compound solution (D2) was changed to 1.56 g. Using the obtained colored composition, peeling evaluation was performed by the above method, and no pattern peeling was observed. In addition, color mixing evaluation was performed by the above method, and T1 / T0 was 0.95. In addition, pin unevenness evaluation was performed by the above method, and unevenness due to the base was confirmed. In addition, color transfer evaluation was performed by the above method, and Y1 / Y0 was 1.00. Comparative Example 5 A colored composition (H13) was prepared in the same manner as in Example 1, except that the amount of binder resin solution (B1) obtained in Production Example 4 was changed to 2.16 g, the amount of radical polymerizable compound (D1) was changed to 2.44 g, and the amount of radical polymerizable compound solution (D2) was changed to 1.05 g. The obtained colored composition was used to perform peeling evaluation by the above method, and no pattern peeling was observed. In addition, when color mixing evaluation was performed by the above method, T1 / T0 was 0.94. In addition, when pin unevenness evaluation was performed by the above method, no unevenness due to the base was observed. In addition, when color transfer evaluation was performed by the above method, Y1 / Y0 was 0.97.

[0100] The amounts of the various additive components added in the above Examples and Comparative Examples are shown in Table 1, and the results of evaluating the resulting colored compositions by the above-mentioned methods are shown in Table 2.

[0101] [Table 1]

[0102] [Table 2]

[0103] Example 9 In a 50 mL plastic bottle, 11.09 g of the dispersion (A1) obtained in Production Example 1, 4.75 g of the dispersion (A2) obtained in Production Example 2, 1.19 g of the binder resin solution (B1) obtained in Production Example 4, 1.07 g of the radical polymerizable compound solution (D1), 3.20 g of the radical polymerizable compound solution (D2), 0.07 g of the photopolymerization initiator (E1), 0.14 g of the photopolymerization initiator (E2), and 23.43 g of the organic solvent propylene glycol monomethyl ether acetate (G1) were added and stirred for 3 hours to prepare a colored composition (H14). When the obtained colored composition was subjected to a peeling evaluation by the above method, no pattern peeling was observed. In addition, when a color mixing evaluation was performed by the above method, T1 / T0 was 0.97. In addition, when a pin unevenness evaluation was performed by the above method, no unevenness due to the pedestal was observed. Furthermore, when color transfer was evaluated by the above-mentioned method, Y1 / Y0 was 0.99. Example 10 In a 50mL plastic bottle, 11.09g of the dispersion (A1) obtained by Production Example 1, 4.75g of the dispersion (A2) obtained by Production Example 2, 1.19g of the binder resin solution (B1) obtained by Production Example 4, 1.07g of the radical polymerizable compound solution (D1), 3.20g of the radical polymerizable compound solution (D2), 0.07g of the photopolymerization initiator (E1), 0.14g of the photopolymerization initiator (E2), 0.11g of the photosensitizer 2,4-diethylthioxanthone (F1), and 23.43g of the organic solvent propylene glycol monomethyl ether acetate (G1) were added and stirred for 3 hours to prepare a colored composition (H15). When the obtained colored composition was evaluated for peeling by the above method, no pattern peeling was observed. In addition, when the color mixing evaluation was performed by the above method, T1 / T0 was 0.98. Furthermore, when pin unevenness was evaluated by the above-mentioned method, unevenness due to the base was not confirmed. Furthermore, when color transfer was evaluated by the above-mentioned method, Y1 / Y0 was 0.99. Example 11 In a 50mL plastic bottle, 11.09g of the dispersion (A1) obtained by Production Example 1, 4.75g of the dispersion (A2) obtained by Production Example 2, 1.19g of the binder resin solution (B1) obtained by Production Example 4, 1.07g of the radical polymerizable compound solution (D1), 3.20g of the radical polymerizable compound solution (D2), 0.07g of the photopolymerization initiator (E1), 0.14g of the photopolymerization initiator (E2), 0.15g of the photosensitizer 2,4-diethylthioxanthone (F1), and 23.43g of the organic solvent propylene glycol monomethyl ether acetate (G1) were added and stirred for 3 hours to prepare a colored composition (H16). When the obtained colored composition was evaluated for peeling by the above method, no pattern peeling was observed. In addition, when the color mixing evaluation was performed by the above method, T1 / T0 was 0.97. Furthermore, when pin unevenness was evaluated by the above-mentioned method, no unevenness due to the base was confirmed. Furthermore, when color transfer was evaluated by the above-mentioned method, Y1 / Y0 was 0.98.

[0104] The amounts of each additive component added in the above examples are shown in Table 3, and the results of evaluating each of the resulting colored compositions by the above-mentioned methods are shown in Table 4.

[0105] [Table 3]

[0106] [Table 4] [Industrial Applicability]

[0107] The colored composition of the present invention can be suitably used for color filter substrates, display devices, decorative ink materials, and the like.

Claims

1. 1. A coloring composition comprising a colorant, a binder resin, a radically polymerizable compound, a photopolymerization initiator and an organic solvent, wherein the radically polymerizable compound comprises dipentaerythritol hexa(meth)acrylate and pentaerythritol tri(meth)acrylate, a ratio of a weight (A) of the dipentaerythritol hexa(meth)acrylate to a weight (B) of the pentaerythritol tri(meth)acrylate is 0.16<A / B<3, and a ratio of a weight (P) of components excluding the colorant, the radically polymerizable compound, the photopolymerization initiator and the organic solvent to a weight (R) of the radically polymerizable compound is 0.5<P / R<0.

9.

2. The colored composition according to claim 1, wherein the photopolymerization initiator is a photopolymerization initiator having a partial structure represented by the following general formula (1), a photopolymerization initiator represented by the following general formulas (2) to (5), or a photopolymerization initiator other than 2,2'-bis(o-chlorophenyl)-4,4',5,5'-tetraphenylbiimidazole. 【Chemistry 1】 In general formula (1), R 3 , and R 4 R each independently represents a hydrogen atom, an alkyl group, an alkenyl group, an alkynyl group, an aryl group, a heteroaryl group, or an alkoxy group. 3 and R 4 may form a ring together. X is OR 5 , S.R. 6 , or N.R. 17 R 18 Indicates the following. 5 , R 6 , R 17 , and R 18 R each independently represents a hydrogen atom, an alkyl group, an alkenyl group, an alkynyl group, an aryl group, or a heteroaryl group. 17 and R 18 may form a ring directly or via a divalent linking group. 【Chemistry 2】 【Chemistry 3】 【Chemistry 4】 【Chemistry 5】

3. 3. The colored composition according to claim 1, wherein the number of moles M of double bonds contained per gram of solid content T excluding the colorant satisfies 160<T / M<220.

4. The coloring composition according to any one of claims 1 to 3, wherein the coloring material comprises a diketopyrrolopyrrole pigment having a bromine group.

5. The colored composition according to any one of claims 1 to 4, wherein the total content of dipentaerythritol hexa(meth)acrylate and pentaerythritol tri(meth)acrylate in the radical polymerizable compound is 70 mass% or more.

6. The colored composition according to any one of claims 1 to 5, further comprising a photosensitizer.

7. 7. The colored composition according to claim 6, wherein the photosensitizer is a thioxanthone-based sensitizer.

8. The colored composition according to claim 6 or 7, wherein a ratio of a weight (P) of components excluding the colorant, the radical polymerizable compound, the photopolymerization initiator, the organic solvent, and the photosensitizer to a weight (R) of the radical polymerizable compound is 0.5<P / R<0.

9.

9. 9. The colored composition according to claim 6, wherein the ratio of the weight (K) of the photosensitizer to the weight (L) of the photopolymerization initiator is 0.3<K / L<0.

6.

10. A color filter substrate having pixels formed from a photocured product of the colored composition according to any one of claims 1 to 9.

11. The color filter substrate according to claim 10, wherein the substrate is a film.

12. A method for producing a color filter substrate, comprising the steps of: (A) applying the colored composition according to any one of claims 1 to 9 onto a substrate; (B) forming a pattern by exposure and development; and (C) further exposing the formed pattern to light.

13. A display device comprising the color filter substrate according to claim 10.

Citation Information

Patent Citations

  • Green colored composition for color filter and color filter

    JP2011022371A

  • Photopolymerizable composition, color filter, method for producing the same, solid-state image pickup element, liquid crystal display device, lithographic printing original plate, and novel compound

    JP2011081349A

  • Colored composition for color filter, and color filter

    JP2012212051A

  • Resin composition, color filter substrate and display device

    JP2016176058A

  • Color filter and display device

    JP2018025681A