Insulating coated electrical steel sheet
The electrical steel sheet with a Zr and Mn-based insulating coating addresses cracking and sticking issues during annealing, ensuring durability and performance in motors and transformers.
Patent Information
- Application Number
- JP2024516549
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-12-02
- Filing Date
- 2023-11-29
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-11-29
AI Technical Summary
Conventional electrical steel sheets with insulating coatings face issues of cracking after strain relief annealing and poor sticking resistance, leading to potential peeling and increased iron loss due to sheet adhesion during annealing.
The insulating coating on the electrical steel sheet contains Zr and Mn, with specific mass ratios of Mn/Zr, optionally with Si and P, and an organic resin, to enhance bonding and prevent cracking and sticking during annealing.
The coating effectively suppresses cracking and ensures excellent sticking resistance, maintaining adhesion and corrosion resistance even at high annealing temperatures.
Smart Images

Figure 0007593531000001 
Figure 0007593531000002 
Figure 0007593531000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an electrical steel sheet with an insulating coating. [Background technology]
[0002] Insulating coatings for magnetic steel sheets used in motors, transformers, etc., are required to have various properties, such as interlaminar resistance, convenience during processing and molding, and stability during storage and use. In particular, insulating coatings with excellent punchability can reduce the number of times dies need to be replaced during punching. Since magnetic steel sheets are used for a variety of purposes, various insulating coatings have been developed according to the purpose. In addition, when magnetic steel sheets are subjected to punching, shearing, bending, etc., residual strain causes deterioration of the magnetic properties, so in order to eliminate this, they are often subjected to stress relief annealing at temperatures of about 700 to 800°C. Therefore, in this case, the insulating coating must be able to withstand stress relief annealing.
[0003] The insulating coating of electromagnetic steel sheets can be broadly divided into (1) Inorganic coating that emphasizes weldability and heat resistance and can withstand stress relief annealing. (2) Resin-containing inorganic coating (i.e., semi-organic coating) that can withstand stress relief annealing in order to achieve both punchability and weldability; (3) Organic coatings for special purposes that cannot be annealed for distortion relief Among these, the coatings that can withstand stress relief annealing as general-purpose products are those containing inorganic components as shown in (1) and (2) above, both of which generally contain chromium compounds. In particular, chromium-based insulating coatings of type (2) are widely used because they can be manufactured in a one-coat, one-bake process, and therefore have significantly improved punchability compared to inorganic insulating coatings.
[0004] However, in recent years, environmental awareness has increased, and in the field of electrical steel sheets, chromate-free products with insulating coatings that do not contain chromium compounds are desired by customers etc. The following are technologies for forming insulating coatings that fall under the above (2) by applying a surface treatment liquid that does not contain chromium compounds and that contains both organic and inorganic components to the surface of electrical steel sheets.
[0005] Patent Document 1 describes a method for manufacturing a magnetic steel sheet comprising: "an electrical steel sheet; and an insulating coating formed on at least one side of the electrical steel sheet, the insulating coating containing Zr and an organic resin, the organic resin having an average primary particle size of 1.0 μm or less, the proportion of primary particles that are aggregated particles being 5% or more and 50% or less of the primary particles of the organic resin, and a total coating weight of the insulating coating on one side of the magnetic steel sheet being 0.1 g / m or less." 2 More than 1.5g / m 2 The document describes an insulating coated electrical steel sheet (Claim 1) characterized by the following: The insulating coated electrical steel sheet described in Patent Document 1 is excellent in both punchability and powder blowing resistance even though the insulating coating does not contain chromium compounds. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2017-160536 A Summary of the Invention [Problem to be solved by the invention]
[0007] However, in conventional electrical steel sheets with an insulation coating, such as that described in Patent Document 1, there is a risk of cracks occurring in the insulation coating after stress relief annealing. If cracks occur in the insulation coating, it is thought that the adhesion of the coating will decrease due to a decrease in the bonding strength within the coating. If the adhesion of the coating decreases due to a decrease in the bonding strength within the coating, the insulation coating may peel off, causing various problems.
[0008] Furthermore, if electrical steel sheets stick to each other during stress relief annealing, an electrical short circuit occurs, causing a problem of increased iron loss. For this reason, electrical steel sheets with an insulating coating are required to not stick to each other during stress relief annealing, i.e., to have excellent sticking resistance.
[0009] In view of the above problems, an object of the present invention is to provide an electrical steel sheet with an insulation coating in which cracking of the insulation coating is suppressed after stress relief annealing and which also has excellent sticking resistance. [Means for solving the problem]
[0010] As a result of intensive research conducted by the present inventors in order to achieve this object, it was discovered that, in an insulating coating containing a Zr compound, when the Mn in the insulating coating is in a certain range in terms of mass ratio Mn / Zr, cracking of the insulating coating after stress relief annealing can be suppressed and excellent sticking resistance can be achieved.
[0011] The gist and configuration of the present invention, which has been completed based on the above findings, is as follows. [1] An electrical wiring board comprising an electrical steel sheet and an insulating coating formed on at least one surface of the electrical steel sheet, 1. An electrical steel sheet with an insulation coating, wherein the insulation coating contains Zr and Mn, and a mass ratio Mn / Zr in the insulation coating is 0.010 or more and 0.100 or less.
[0012] [2] The electrical steel sheet with an insulation coating according to the above [1], wherein the insulation coating contains Si and has a mass ratio Si / Zr of 1.5 or less.
[0013] [3] The electrical steel sheet with an insulation coating according to the above [1] or [2], wherein the insulation coating contains P and has a mass ratio P / Zr of 1.5 or less in the insulation coating.
[0014] [4] The electrical steel sheet with an insulation coating according to any one of the above [1] to [3], wherein the insulation coating contains an organic resin, and the organic resin (mass %) / Zr calculated as ZrO2 (mass %) in the insulation coating is 0.5 or less.
[0015] [5] A motor having an iron core formed by laminating the electrical steel sheets with an insulating coating according to any one of [1] to [4] above.
[0016] [6] A transformer having an iron core formed by laminating the insulating coating-coated electrical steel sheets according to any one of [1] to [4] above. Effect of the Invention
[0017] The electrical steel sheet with an insulating coating of the present invention is inhibited from cracking in the insulating coating after stress relief annealing, and also has excellent sticking resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] An electrical steel sheet with an insulating coating according to one embodiment of the present invention comprises an electrical steel sheet and an insulating coating formed on at least one side of the electrical steel sheet.
[0019] [Electromagnetic steel sheet] The electromagnetic steel sheet (base steel sheet) that serves as the base of the insulating coating is not limited to a specific electromagnetic steel sheet. For example, an electromagnetic steel sheet having a general composition can be used. General components include Si, Mn, Al, etc., with the balance being Fe and unavoidable impurities. Usually, the Si content is 0.05 to 7.0 mass%, the Mn content is 0.05 to 10.0 mass%, and the Al content is 2.0 mass% or less.
[0020] The type of electrical steel sheet is not particularly limited, and any of so-called soft iron sheets (electrical steel sheets) with high magnetic flux density, general cold-rolled steel sheets such as SPCC, non-oriented electrical steel sheets containing Si or Al to increase resistivity, etc. Non-oriented electrical steel sheets conforming to JIS C2552:2014 and oriented electrical steel sheets conforming to JIS C2553:2019 can be preferably used.
[0021] [Insulating coating] In this embodiment, the insulating coating contains Zr and Mn, and optionally further contains one or more selected from the group consisting of Si, P, and an organic resin. The components contained in the insulating coating will be described below.
[0022] The insulating coating containing Zr can be formed by using a Zr compound as a raw material. Examples of Zr compounds include zirconium acetate, zirconium oxide, zirconium propionate, zirconium oxychloride, zirconium nitrate, ammonium zirconium carbonate, potassium zirconium carbonate, zirconium hydroxychloride, zirconium sulfate, potassium zirconium hexafluoride, tetra-normal propoxy zirconium, tetra-normal butoxy zirconium, zirconium tetraacetylacetonate, zirconium tributoxy acetylacetonate, zirconium tributoxy stearate, and the like. In this embodiment, one or more selected from these can be used. Such Zr compounds have a strong bond with oxygen and can be firmly bonded to oxides, hydroxides, and the like on the surface of the electrical steel sheet. In addition, since Zr has three or more bonds, a network can be formed between Zr or with other inorganic compounds, thereby forming a tough insulating coating without containing a chromium compound.
[0023] The amount of Zr compound attached (Zr content in the insulation coating) is 0.05 g / m2 in terms of ZrO2. 2 In the above cases, the ZrO2 coating is sufficient, improving corrosion resistance. In addition, the amount of Zr compound attached (Zr content in the insulation coating) is 1.50 g / m2 in terms of ZrO2. 2 In the following cases, cracks in the insulation coating are unlikely to occur, and the coating adhesion and corrosion resistance are good. Therefore, the amount of Zr compound attached (Zr content in the insulation coating) should be 0.05 g / m2 in terms of ZrO2. 2 More than 1.50g / m 2 It is preferable to adjust the Zr content in the insulating coating to the following value. It is considered that the Zr compound as the raw material is entirely converted to ZrO2 in the insulating coating. In other words, it is considered that the Zr in the insulating coating exists as ZrO2. For this reason, in this embodiment, the Zr content in the insulating coating is calculated as the amount converted to ZrO2. The amount converted to ZrO2 (g / m 2 ) can be calculated from the following formula: ZrO2 equivalent amount (g / m 2 )=film adhesion amount (g / m 2)×ZrO2 equivalent amount (mass%) / 100 The coating weight is calculated by measuring the weight of the electrical steel sheet before the insulating coating is formed and the weight of the electrical steel sheet with the insulating coating. The coating weight is 0.05 g / m 2 More than 1.50g / m 2 It is preferable that the coating weight is 0.05 g / m or less. 2 If the coating thickness is more than 1.50g / m, corrosion resistance can be ensured. 2 If it is below this value, the coating adhesion can be ensured. The ZrO2 equivalent (mass%) is determined by measuring the Zr content (mass%) in the coating portion using energy dispersive X-ray spectroscopy (EDX) analysis with a transmission electron microscope and converting this to the ZrO2 equivalent (mass%). It is desirable to analyze about 10 points and use the average value.
[0024] The insulating coating containing Mn can be formed by using a Mn compound as a raw material. Examples of Mn compounds include MnO2 and Mn2O3, and one or both of these can be used.
[0025] In this embodiment, it is important that the mass ratio Mn / Zr in the insulating coating is 0.010 or more and 0.100 or less.
[0026] When the mass ratio Mn / Zr is 0.010 or more, the Mn content in the insulating coating is sufficient, and the effect of suppressing cracking of the insulating coating after stress relief annealing can be obtained. Although it is not clear why cracking can be suppressed when the mass ratio Mn / Zr is 0.010 or more, the inventors believe that the root cause is high reactivity between Zr compounds and Mn. In other words, when the mass ratio Mn / Zr is 0.010 or more, it is believed that a chemical reaction is likely to occur in the insulating coating, bonds are formed between molecules, and as a result, cracking is suppressed.
[0027] On the other hand, if the mass ratio Mn / Zr exceeds 0.100, the magnetic steel sheets are stuck together during stress relief annealing, resulting in poor sticking resistance. This is thought to be because the insulating coating applied to the magnetic steel sheets is highly reactive, forming new chemical bonds between the laminated magnetic steel sheets, resulting in sticking. Therefore, from the viewpoint of obtaining excellent sticking resistance, the mass ratio Mn / Zr is set to 0.100 or less, preferably 0.050 or less. Here, in the past, stress relief annealing was often performed at a temperature of about 700 to 800 ° C., but recently, in order to further improve magnetic properties, stress relief annealing has been aimed at increasing the temperature, and stress relief annealing at a temperature of about 900 ° C. has been considered. In this embodiment, by setting the mass ratio Mn / Zr to 0.100 or less, a remarkable effect of excellent sticking resistance in stress relief annealing at a high temperature of 900 ° C. is achieved.
[0028] In the present embodiment, the insulating coating may contain Si from the viewpoint of improving insulation. The insulating coating containing Si can be formed by using a Si compound as a raw material. Examples of the Si compound include colloidal silica, fumed silica, alkoxysilane, and siloxane, and one or more selected from these can be used. From the viewpoint of obtaining a sufficient effect of improving insulation, the mass ratio Si / Zr in the insulating coating is preferably 0.5 or more. Furthermore, from the viewpoint of suppressing a decrease in coating adhesion due to a decrease in the bonding strength between the magnetic steel sheet and the insulating coating, the mass ratio Si / Zr in the insulating coating is preferably 1.5 or less.
[0029] In the present embodiment, the insulating coating may contain P from the viewpoint of improving corrosion resistance. The insulating coating containing P can be formed by using a P compound as a raw material. Examples of the P compound include phosphoric acids such as orthophosphoric acid, phosphoric anhydride, linear polyphosphoric acid, and cyclic metaphosphoric acid, and phosphates such as ammonium phosphate, magnesium phosphate, aluminum phosphate, calcium phosphate, and zinc phosphate, and one or more selected from these can be used. From the viewpoint of fully obtaining the effect of improving corrosion resistance, the mass ratio P / Zr in the insulating coating is preferably 0.5 or more. Furthermore, from the viewpoint of suppressing a decrease in coating adhesion due to a decrease in the bonding strength between the magnetic steel sheet and the insulating coating, the mass ratio P / Zr in the insulating coating is preferably 1.5 or less.
[0030] In this specification, the mass ratios Mn / Zr, Si / Zr, and P / Zr in the insulating coating are determined by the following method.
[0031] First, the mass ratio Mn / Zr in the insulating coating is measured by Auger electron spectroscopy. While ion sputtering, a depth profile is performed by Auger electron spectroscopy so that at least Mn, Zr, Si, P, Fe, O, and C are included in the measurement elements, and a depth profile is created by converting the signal intensity ratio of each element into a mass concentration. The average mass concentration of Mn and Zr is calculated from the depth where the mass concentration of Zr is reduced to half from the maximum point when analyzed in the depth direction from the sputtering start point, and the average value of the Mn mass concentration is divided by the average value of the Zr mass concentration. At this time, the number of analysis points on the insulating coating is 10 or more, and the average value of the average Mn mass concentration / average Zr mass concentration of all analysis points is defined as the "mass ratio Mn / Zr" in the present invention. The depth where the mass concentration of Zr is reduced to half is defined as the "insulating coating". Needless to say, the part deeper than the position where the mass concentration of Zr is reduced to half is the "electromagnetic steel sheet".
[0032] The mass ratios Si / Zr and P / Zr in the insulating coating are also measured by Auger electron spectroscopy. That is, the mass ratios Si / Zr and P / Zr can be obtained by replacing the Mn mass concentration in the previous paragraph with the Si mass concentration and the P mass concentration, respectively.
[0033] In the present embodiment, the insulating coating may contain an organic resin from the viewpoint of improving various coating properties such as corrosion resistance and punchability. There are no particular limitations on the organic resin, and any known or arbitrary resin may be used. Examples of the organic resin include aqueous resins (emulsions, dispersions, water-soluble resins) such as acrylic resins, alkyd resins, polyolefin resins, styrene resins, vinyl acetate resins, epoxy resins, phenolic resins, polyester resins, urethane resins, and melamine resins, and one or more selected from these may be used.
[0034] From the viewpoint of sufficiently improving the coating performance, it is preferable that the ratio of organic resin (mass %) / Zr converted into ZrO2 (mass %) in the insulating coating is 0.05 or more. On the other hand, since organic resin is more permeable to oxygen than Zr compounds, if there is too much organic resin, the corrosion resistance deteriorates. From this viewpoint, it is preferable that the ratio of organic resin (mass %) / Zr converted into ZrO2 (mass %) in the insulating coating is 0.5 or less.
[0035] The ZrO2 equivalent amount (mass %) of organic resin (mass %) / Zr in the insulating coating is determined by the following method. The C and Zr contents (mass %) of the coating are measured by EDX analysis using a transmission electron microscope. The ZrO2 equivalent amount (mass %) of organic resin (mass %) is determined by converting the C content (mass %) to organic resin content (mass %), converting the Zr content (mass %) to ZrO2 equivalent amount (mass %), and dividing the organic resin content (mass %) by the ZrO2 equivalent amount (mass %). It is desirable to analyze around 10 points and use the average value.
[0036] In the present embodiment, the insulating coating preferably comprises a Zr compound serving as a Zr source, a Mn compound serving as a Mn source, and optionally one or more selected from the group consisting of a Si compound serving as a Si source, a P compound serving as a P source, and an organic resin, and optionally further comprises other components described below.
[0037] Furthermore, in this embodiment, in addition to the above-mentioned components, the inclusion of commonly used additives such as surfactants, rust inhibitors, lubricants, and antioxidants, inorganic compounds such as boric acid and pigments, and organic compounds is not prevented. The organic compound may contain an organic acid as a contact inhibitor between the inorganic component and the organic resin. Examples of organic acids include polymers or copolymers containing acrylic acid. These other components can be added to an extent that does not impair the effects of the present invention, but if the total solid content (mass%) of the additives / ZrO2 equivalent (mass%) exceeds 1.0, unreacted substances remain in the coating film and reduce water resistance, so the content is preferably 1.0 or less, preferably 0.5 or less, in terms of the total solid content (mass%) of the additives / ZrO2 equivalent (mass%).
[0038] In this embodiment, impurities such as Hf, HfO2, and TiO2 may be mixed into the inorganic components. However, as long as the total amount of these impurities is 5 mass % or less based on the amount of ZrO2, no particular problem occurs.
[0039] The method for producing an electrical steel sheet with an insulating coating is described below. There are no particular limitations on the pretreatment of the electrical steel sheet. That is, the electrical steel sheet may be untreated, but it is advantageous to subject the sheet to a degreasing treatment using an alkali or the like, or an acid pickling treatment using hydrochloric acid, sulfuric acid, phosphoric acid, or the like.
[0040] Next, a treatment liquid for forming an insulating coating is prepared by adding the Zr compound, the Mn compound, optionally one or more selected from the group consisting of the Si compound, the P compound, and the organic resin, and optionally further the other components, to deionized water and mixing them.
[0041] The treatment solution is then applied to the surface of the electrical steel sheet by any method, including roll coating, bar coating, immersion, spray coating, etc., and the most suitable method is selected depending on the shape of the electrical steel sheet to be treated, etc.
[0042] Next, the treatment liquid applied to the magnetic steel sheet is baked to form the applied treatment liquid into an insulating coating. The baking method is not particularly limited, and commonly used methods such as hot air heating, infrared heating, and induction heating can be used. The maximum sheet temperature is not particularly limited, and may be about 150 to 350°C. The heating time is not particularly limited, and may be appropriately set within a range of 1 second to 10 minutes.
[0043] Through the above steps, the electrical steel sheet with an insulation coating according to this embodiment can be manufactured.
[0044] It is preferable to form the insulating coating on both sides of the electromagnetic steel sheet, but it may be formed on only one side depending on the purpose. Also, depending on the purpose, the insulating coating of this embodiment may be formed on one side of the electromagnetic steel sheet and another insulating coating may be formed on the other side.
[0045] The electrical steel sheet with the insulation coating of this embodiment can be subjected to stress relief annealing to remove stress due to punching, for example. As a preferred stress relief annealing atmosphere, an atmosphere in which iron is not easily oxidized, such as an N2 atmosphere or a DX gas atmosphere, is used. Here, the corrosion resistance can be further improved by setting the dew point high, for example, Dp: about 5 to 60°C, and slightly oxidizing the surface and the cut end surface. In addition, the generally preferred stress relief annealing temperature is 700 to 900°C, more preferably 700 to 800°C, but the insulation coating of this embodiment can be subjected to stress relief annealing even at 900°C. The holding time at the stress relief annealing temperature is preferably long, more preferably 1 hour or more.
[0046] A motor according to one embodiment of the present invention is characterized in that it has an iron core formed by stacking the above-mentioned insulating coated magnetic steel sheets. Also, a transformer according to one embodiment of the present invention is characterized in that it has an iron core formed by stacking the above-mentioned insulating coated magnetic steel sheets.
[0047] That is, the electrical steel sheet with an insulating coating of this embodiment is suitable for use, for example, in the rotor core of a motor with built-in permanent magnets (IPM motor). In recent years, the drive motors used in hybrid electric vehicles (HEVs) and electric vehicles (EVs) have become much faster, and during high-speed rotation, strong centrifugal forces act on the bridge parts in which the permanent magnets are embedded. The electrical steel sheet with an insulating coating of this embodiment can withstand such centrifugal forces. Note that the application of the electrical steel sheet with an insulating coating of this embodiment is not limited to rotor cores, and it can also be used, for example, in the core of a stator (fixed part) or the like.
[0048] Using the same insulating coated steel sheet for both the rotor core component and the stator core component is advantageous in terms of yield, since the approximately circular region in the center of the stator core component, which is punched out into an approximately annular shape, can be used as the material for the rotor core component; this type of cutting is known as "common cutting" and is common.
[0049] It is preferable to perform stress relief annealing on a member punched from an insulating coated steel sheet for use as a stator core, or a stator core formed by laminating such a member. Since high strength is not required for a material for a stator core, and low core loss is important, it is preferable to release processing strain that adversely affects core loss.
[0050] Whether the steel sheets are for rotor cores or stator cores, assuming that they are to be produced in the same process, stress relief annealing is carried out to remove the processing strain imposed on the electromagnetic steel sheet when the insulating coated steel sheet is punched out, and according to the present invention, an electromagnetic steel sheet with good sticking resistance can be obtained.
[0051] Hereinafter, the present invention will be described in more detail with reference to examples, but the present invention is not limited to the following examples at all.
Example
[0052] In each of the test examples shown in Table 1, a Zr compound, a Mn compound, and in some examples, one of a Si compound, a P compound, and an organic resin were added to deionized water and mixed to prepare a treatment liquid. In Table 1, Z1 to Z4 representing the Zr compound are shown in Table 2, M1 and M2 representing the Mn compound are shown in Table 3, S1 representing the Si compound is shown in Table 4, P1 representing the P compound is shown in Table 5, and R1 and R2 representing the organic resin are shown in Table 6. The total solid content concentration of each component with respect to the amount of deionized water was 50 g / L.
[0053] In each test example, on one side of a test piece cut out from an electromagnetic steel sheet (A360 (JIS C 2552 (2000))) with a plate thickness of 0.35 mm to a size of width: 150 mm and length: 300 mm, the treatment liquid was applied with a roll coater and baked in a hot air baking furnace at a maximum plate temperature of 200 °C for a heating time of 30 seconds. Then, it was allowed to cool to room temperature to obtain an insulating film with a film adhesion amount of 0.50 g / m 2 of the insulating film.
[0054] <ZrO2 equivalent amount (mass %) and ZrO2 equivalent amount (mass ratio)> By EDX analysis using a transmission electron microscope, the Zr content (mass %) of the film portion was measured and converted to the ZrO2 equivalent amount (mass %). Note that when Zr is baked on the steel sheet to form the insulating film, it undergoes a chemical reaction and the entire amount exists in the insulating film as ZrO2. Therefore, the Zr content is calculated assuming it is the ZrO2 equivalent amount. The number of analysis points was 10, and the average value was shown as "ZrO2 equivalent amount (mass %)" in Table 1. Also, the contents (mass %) of Z1 to Z4 in Table 1 are also the ZrO2 equivalent amounts (mass %) of each Zr compound in the insulating film and were obtained by the same method. The ZrO2 equivalent amount (mass ratio) was obtained by ZrO2 equivalent amount (mass %) / 100 and shown in Table 1.
[0055] <Amount of ZrO2 equivalent (g / m 2 )> The amount of ZrO2 equivalent (g / m 2 ) was determined by the above-described method, and the values are shown in Table 1.
[0056] <Contents of Mn compound, Si compound, P compound, and organic resin (mass%)> The contents (mass%) of M1 and M2 in Table 1 are the amounts of Mn equivalent to MnO2 or Mn2O3 in the insulating film. By EDX analysis using a transmission electron microscope, the Mn content (mass%) of the film portion was measured and converted to the amount of MnO2 equivalent or Mn2O3 equivalent (mass%). The content (mass%) of S1 in Table 1 is the amount of Si equivalent to SiO2 in the insulating film. By EDX analysis using a transmission electron microscope, the Si content (mass%) of the film portion was measured and converted to the amount of SiO2 equivalent (mass%). The content (mass%) of P1 in Table 1 is the amount of P equivalent to PO4 in the insulating film. By EDX analysis using a transmission electron microscope, the P content (mass%) of the film portion was measured and converted to the amount of PO4 equivalent (mass%). The contents (mass%) of R1 and R2 in Table 1 are the contents of the organic resin in the insulating film. By EDX analysis using a transmission electron microscope, the C content (mass%) of the film portion was measured and converted to the organic resin content (mass%). In all cases, the number of analysis points was 10, and the average value was adopted. In the EDX analysis using the transmission electron microscope of this example, the acceleration voltage was 200 kV in all cases.
[0057] <Mass ratios of Mn / Zr, Si / Zr, and P / Zr> Analysis was performed using an Auger electron spectrometer (manufactured by PHISICAL ELECTONICS Co., Ltd.) at an acceleration voltage of 10 kV and a sample current of 0.2 μA. Depth analysis was performed at a sputter rate of 3 nm / min (value for ZrO2), measured every 2 min, and measured until the Zr count reached the noise level. Based on the results of this analysis, the mass ratios of Mn / Zr, Si / Zr, and P / Zr were calculated by the above-described method, and the respective values are shown in Table 1.
[0058] <Organic resin (mass%) / ZrO2 equivalent (mass%) The ZrO2 equivalent amount (mass %) of organic resin (mass %) / Zr was determined by the method described above, and the values are shown in Table 1.
[0059] The electrical steel sheets with insulation coating obtained in each test example were subjected to the following evaluations, and the results are shown in Table 1.
[0060] <Cracks in the insulating coating> The surface of the insulating coating was observed using a scanning electron microscope (ULTRA PLUS manufactured by Carl Zeiss) at an accelerating voltage of 5 kV to determine the presence or absence of cracks in the insulating coating. The magnification during observation was 1000 times. ◎ and ○ were deemed to be acceptable. (Judgment criteria) ◎: No cracks ○: Some cracks ×: Cracks on the entire surface
[0061] <Anti-sticking> Ten 50mm square test pieces are stacked together and the load is 20kPa (200g / cm 2 The specimens were annealed at 900°C for 2 hours in a nitrogen atmosphere while applying a 500g pressure. A 500g weight was then dropped onto the specimens, and the drop height at which the 10 bonded specimens were divided into 5 was measured. The lower the drop height, the better the sticking resistance. ◎ and ○ were deemed to be acceptable. (Judgment criteria) ◎: 10cm or less ○: More than 10cm, less than 15cm △: More than 15cm, less than 30cm ×: More than 30cm
[0062] <Adhesion> Scotch tape (registered trademark) was applied to the surface of the test material, and the material was bent inward by Φ10 mm, after which the Scotch tape was peeled off and the remaining state of the insulating coating was observed to evaluate the adhesion of the insulating coating to the magnetic steel sheet. (Judgment criteria) ◎: Survival rate 90% or more ○: Residual rate 60% or more, less than 90% △: Residual rate 30% or more, less than 60% ×: Residual rate less than 30%
[0063] <Corrosion resistance> The test specimens were subjected to a humidity test (50°C, relative humidity ≧98%), and the incidence of red rust after two weeks was observed and evaluated based on the area ratio. (Judgment criteria) ◎: Red rust area ratio less than 20% ○: Red rust area ratio 20% or more, less than 40% △: Red rust area ratio 40% or more, less than 60% ×: Red rust area ratio 60% or more
[0064] [Table 1] TIFF0007593531000002.tif233148
[0065] [Table 2]
[0066] [Table 3]
[0067] [Table 4]
[0068] [Table 5]
[0069] [Table 6] [Industrial Applicability]
[0070] INDUSTRIAL APPLICABILITY The electrical steel sheet with an insulating coating of the present invention is extremely useful as parts for motors, transformers, etc., since cracking of the insulating coating is suppressed after stress relief annealing and the electrical steel sheet has excellent sticking resistance.
Claims
1. An electrical steel sheet and an insulating coating formed on at least one surface of the electrical steel sheet, 1. An electrical steel sheet with an insulation coating, wherein the insulation coating contains a Zr compound and a Mn compound, and a mass ratio Mn / Zr in the insulation coating is 0.010 or more and 0.100 or less.
2. 2. The electrical steel sheet with an insulation coating according to claim 1, wherein the insulation coating contains Si, and a mass ratio Si / Zr in the insulation coating is 1.5 or less.
3. 2. The electrical steel sheet with an insulation coating according to claim 1, wherein the insulation coating contains P, and a mass ratio P / Zr in the insulation coating is 1.5 or less.
4. 3. The electrical steel sheet with an insulation coating according to claim 2, wherein the insulation coating contains P, and a mass ratio P / Zr in the insulation coating is 1.5 or less.
5. The insulating coating contains an organic resin, and the organic resin (mass %) / Zr in the insulating coating is ZrO 2 The electrical steel sheet with an insulation coating according to any one of claims 1 to 4, wherein the converted amount (mass%) is 0.5 or less.
6. A motor having an iron core formed by laminating the insulating coated electrical steel sheets according to any one of claims 1 to 4.
7. A motor having an iron core formed by laminating the insulating coated electrical steel sheets according to claim 5.
8. A transformer having an iron core formed by laminating the insulating coated electrical steel sheets according to any one of claims 1 to 4.
9. A transformer having an iron core formed by laminating the insulating-coated magnetic steel sheets according to claim 5.
Citation Information
Patent Citations
Electrical insulation coating sheet treatment agent for directive electro-magnetic steel sheet, directive electro-magnetic steel sheet, and electrical insulation coating sheet treatment method for directive electro-magnetic steel sheet
JP2017137540A
Magnetic steel sheet with electrical insulation coating sheet
JP2017160536A
Electromagnetic steel sheet having insulating coating film attached thereto
WO2014188679A1
Insulating coating treatment solution, and grain oriented electrical steel sheet having insulating coating film attached thereto and method for manufacturing same
WO2020026627A1
Electrically insulating coating for anisotropic electrical steel
WO2022255910A1