Electrical inspection device, manufacturing method and electrical current supply method for semiconductor device
A current testing device with a variable thermal resistance mechanism addresses the inefficiencies in silicon carbide power MISFET screening by allowing simultaneous on-voltage and leakage current measurement, reducing screening time and ensuring consistent quality assessment.
Patent Information
- Application Number
- JP2023508830
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-03-24
- Filing Date
- 2022-02-24
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2042-02-24
AI Technical Summary
Current testing devices for silicon carbide power MISFETs face challenges in maintaining accuracy and efficiency during the screening process due to fixed thermal resistance values, leading to increased screening time and variability with changing product specifications, and the inability to accurately measure both on-voltage and leakage current simultaneously.
The implementation of a current testing device with a variable thermal resistance mechanism and a method that includes adjusting thermal resistance to achieve the maximum rated junction temperature, allowing simultaneous measurement of on-voltage and leakage current to determine semiconductor device quality, thereby reducing screening time and ensuring consistent accuracy.
This approach significantly reduces the time required for screening while maintaining consistent accuracy, enabling precise selection of high-quality semiconductor devices by accounting for varying product specifications and preventing potential breakdown failures.
Smart Images

Figure 0007593578000001 
Figure 0007593578000002 
Figure 0007593578000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an electrical inspection device, a manufacturing method for a semiconductor device, and an electrical inspection method, and more particularly to an electrical inspection device for selecting semiconductor devices using silicon carbide substrates, a manufacturing method for a semiconductor device using the electrical inspection device, and an electrical inspection method using the electrical inspection device. [Background technology]
[0002] Metal Insulator Semiconductor Field Effect Transistors (MISFETs), which are one type of power semiconductor device, have traditionally been dominated by power MISFETs using silicon (Si) substrates (Si power MISFETs). However, the electric field strength required for dielectric breakdown in silicon carbide (SiC) is approximately one order of magnitude larger than that in Si.
[0003] Therefore, in a power MISFET using a SiC substrate (SiC power MISFET), the thickness of the drift layer for maintaining the breakdown voltage can be reduced to about 1 / 10 compared to a Si power MISFET, and the impurity concentration of the drift layer can be increased by about 100 times. As a result, in a SiC power MISFET, the element resistance can be theoretically reduced by three orders of magnitude or more. In addition, since SiC has a band gap about three times larger than that of Si, the SiC power MISFET can reduce the on-resistance at the same breakdown voltage and can also operate in a high-temperature environment. For this reason, the SiC power MISFET is expected to have performance that exceeds that of a Si power MISFET.
[0004] In addition, a vertical planar structure may be applied to a SiC power MISFET, in which a drain electrode is provided on the back side of the SiC substrate, and a source electrode and a gate electrode are provided on the front side of the SiC substrate. Such a vertical MISFET includes a parasitic pn diode between the source electrode and the drain electrode as a built-in diode, which is composed of a p-type body region and an n-type SiC epitaxial layer. This built-in diode can be used as a freewheeling diode for an inverter.
[0005] However, n-type SiC substrates may contain defects. In such cases, when a current flows through the built-in diode, electrons and holes recombine inside the n-type SiC substrate or inside the n-type SiC epitaxial layer formed on the n-type SiC substrate. The recombination energy generated at this time moves basal plane dislocations, a type of crystal defect present in the SiC substrate, and stacking faults sandwiched between two basal plane dislocations grow.
[0006] Since stacking faults make it difficult for current to flow, as stacking faults grow, the on-resistance of the SiC power MISFET and the forward voltage of the built-in diode increase. Since stacking faults grow cumulatively, if this operation continues, the loss generated in the inverter circuit increases over time, the amount of heat generated also increases, and this can cause failure of the semiconductor device (semiconductor chip).
[0007] Therefore, an inspection method is used to screen semiconductor devices having SiC power MISFETs and select semiconductor devices that are free or nearly free of stacking faults.
[0008] For example, Patent Document 1 discloses a method in which a forward current is first applied to a built-in diode, a junction temperature of a SiC power MISFET is set, and then an on-voltage Von0 is measured, a forward current is applied to the built-in diode, and an on-voltage Von1 is measured again, and a change in the on-voltage Von0 and the on-voltage Von1 is calculated to determine whether the semiconductor device is unqualified. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] JP 2020-150181 A Summary of the Invention [Problem to be solved by the invention]
[0010] In an electrical inspection device that performs the screening method as described in Patent Document 1, a measuring electrode for applying a drain voltage and a cooling plate for cooling the semiconductor device are usually provided on the drain electrode side of the SiC power MISFET. Also, an insulating plate is provided between the measuring electrode and the cooling plate to electrically insulate the measuring electrode and the cooling plate.
[0011] In a typical electrical inspection device, the thermal resistance value of the structure including the insulating plate is fixed. Therefore, when a forward current is applied to the built-in diode and the maximum rated junction temperature is reached, the forward current cannot be increased any further. This requires a longer current application time to grow stacking faults, which increases the time required for screening semiconductor devices. Furthermore, if the product specifications, such as the maximum rating or the thickness of the semiconductor substrate, change, the defect growth rate also changes, and the screening conditions also change, so the accuracy of screening semiconductor devices cannot be kept constant.
[0012] The main object of the present application is to provide a method for reducing the time required for screening semiconductor devices and for stabilizing the accuracy of sorting semiconductor devices regardless of product specifications. Also, to provide an electrical inspection device that can achieve these. Another object of the present application is to provide a highly reliable semiconductor device 100 by performing precise screening of the semiconductor device 100.
[0013] Other objects and novel features will become apparent from the description of this specification and the accompanying drawings. [Means for solving the problem]
[0014] In one embodiment, the electrical inspection device includes a cooling plate, an insulating plate provided on the cooling plate, a first electrode provided on the insulating plate, and a second electrode and a third electrode provided above the first electrode and positioned apart from the first electrode, where the insulating plate has a variable thermal resistance mechanism, and a semiconductor device can be installed between the first electrode and the second electrode and between the first electrode and the third electrode.
[0015] In one embodiment, a manufacturing method for a semiconductor device uses an electrical conductivity inspection device that includes a cooling plate, an insulating plate provided on the cooling plate and having a variable thermal resistance mechanism, a first electrode provided on the insulating plate, and a second electrode and a third electrode provided above the first electrode and positioned away from the first electrode. A method for manufacturing a semiconductor device includes: (a) preparing a semiconductor device including a drain electrode, a source electrode, and a gate pad electrode; (b) after the step (a), placing the semiconductor device between the first electrode and the second electrode and between the first electrode and the third electrode, electrically connecting the first electrode to the drain electrode, electrically connecting the second electrode to the source electrode, and electrically connecting the third electrode to the gate pad electrode; (c) after the step (b), adjusting a resistance value of the variable thermal resistance mechanism so that a maximum rated junction temperature of the semiconductor device is reached when a maximum rated forward current of the semiconductor device is passed through a built-in diode of the semiconductor device; (d) after the step (c), measuring a first on-voltage of the semiconductor device; and (e) after the step (c), measuring a first on-voltage of the semiconductor device between the source electrode and the drain electrode in a state in which the source electrode and the gate pad electrode are electrically short-circuited or a negative bias is applied to the gate pad electrode with respect to the source electrode. (f) after the steps (d) and (e), passing a forward current through the built-in diode; (g) after the step (f), measuring a second on-voltage of the semiconductor device; (h) after the step (g), calculating a change between the second on-voltage and the first on-voltage, and selecting the semiconductor device as a conforming product if the change is smaller than a specified rate; (i) after the step (h), measuring a second leakage current when a specified voltage is applied between the source electrode and the drain electrode with the source electrode and the gate pad electrode electrically shorted or with a negative bias applied to the gate pad electrode with respect to the source electrode, for the semiconductor device selected as a conforming product; (j) after the step (i), calculating a change between the second leakage current and the first leakage current, and selecting the semiconductor device as a conforming product if the change is smaller than a specified value.Here, the step (a) includes the steps of: (a1) preparing a semiconductor substrate of a first conductivity type having a surface and a back surface opposite to the surface and made of silicon carbide; (a2) forming a semiconductor layer of the first conductivity type made of silicon carbide on the surface of the semiconductor substrate; (a3) forming a body region of a second conductivity type opposite to the first conductivity type in the semiconductor layer; (a4) forming a source region of the first conductivity type in the body region; (a5) forming a gate insulating film on the body region; (a6) forming a gate electrode on the gate insulating film; (a7) forming the source electrode on the body region and the source region so as to be electrically connected to the body region and the source region, and forming the gate pad electrode on the gate electrode so as to be electrically connected to the gate electrode; and (a8) forming the drain electrode on the back surface of the semiconductor substrate. The built-in diode is constituted by the body region and the semiconductor layer.
[0016] In one embodiment, the electrical current method uses an electrical current inspection device that includes a cooling plate, an insulating plate provided on the cooling plate and having a variable thermal resistance mechanism, a first electrode provided on the insulating plate, and a second electrode and a third electrode provided above the first electrode and positioned away from the first electrode. The current application method includes the steps of: (a) preparing a semiconductor device including a drain electrode, a source electrode, and a gate pad electrode; (b) after the step (a), placing the semiconductor device between the first electrode and the second electrode and between the first electrode and the third electrode, electrically connecting the first electrode to the drain electrode, electrically connecting the second electrode to the source electrode, and electrically connecting the third electrode to the gate pad electrode; (c) after the step (b), adjusting a resistance value of the variable thermal resistance mechanism so that a maximum rated junction temperature of the semiconductor device is reached when a maximum rated forward current of the semiconductor device is applied to a built-in diode of the semiconductor device; (d) after the step (c), measuring a first on-voltage of the semiconductor device; and (e) after the step (c), measuring a first on-voltage of the semiconductor device between the source electrode and the drain electrode in a state in which the source electrode and the gate pad electrode are electrically short-circuited or a negative bias is applied to the gate pad electrode with respect to the source electrode. (f) after the steps (d) and (e), passing a forward current through the built-in diode; (g) after the step (f), measuring a second on-voltage of the semiconductor device; (h) after the step (g), calculating a change in value between the second on-voltage and the first on-voltage, and selecting the semiconductor device as a conforming product if the change in value is smaller than a specified rate; (i) after the step (h), measuring a second leakage current when a specified voltage is applied between the source electrode and the drain electrode with the source electrode and the gate pad electrode electrically shorted or with a negative bias applied to the gate pad electrode with respect to the source electrode, for the semiconductor device selected as a conforming product; (j) after the step (i), calculating a change in value between the second leakage current and the first leakage current, and selecting the semiconductor device as a conforming product if the change in value is smaller than a specified value.Here, the semiconductor device includes a semiconductor substrate of a first conductivity type having a surface and a back surface opposite to the surface and made of silicon carbide, a semiconductor layer of the first conductivity type formed on the surface of the semiconductor substrate and made of silicon carbide, a body region of a second conductivity type opposite to the first conductivity type formed in the semiconductor layer, a source region of the first conductivity type formed in the body region, a gate insulating film formed on the body region, a gate electrode formed on the gate insulating film, the source electrode formed on the body region and the source region so as to be electrically connected to the body region and the source region, the gate pad electrode formed on the gate electrode so as to be electrically connected to the gate electrode, and the drain electrode formed on the back surface of the semiconductor substrate. The built-in diode is composed of the body region and the semiconductor layer.
[0017] In one embodiment, a method for manufacturing a semiconductor device includes the steps of: (a) preparing a semiconductor device including a drain electrode, a source electrode, a gate pad electrode, and a built-in diode; (b) after the step (a), measuring a first on-voltage of the semiconductor device; (c) after the step (b), passing a forward current through the built-in diode; (d) after the step (c), measuring a second on-voltage of the semiconductor device; (e) after the step (d), calculating a change in value between the second on-voltage and the first on-voltage, and selecting the semiconductor device as a conforming product if the change in value is smaller than a first specified value; (f) after the step (e), measuring a leakage current when a predetermined voltage is applied between the source electrode and the drain electrode of the semiconductor device selected as a conforming product with the source electrode and the gate pad electrode electrically shorted or with a negative bias applied to the gate pad electrode with respect to the source electrode; and (g) after the step (f), selecting the semiconductor device as a conforming product if the leakage current is smaller than a second specified value.
[0018] In one embodiment, a method for manufacturing a semiconductor device includes: (a) preparing a semiconductor device including a drain electrode, a source electrode, a gate pad electrode, and a built-in diode; (b) measuring a first on-voltage of the semiconductor device after the step (a); (c) measuring a first leakage current when a prescribed voltage is applied between the source electrode and the drain electrode in a state in which the source electrode and the gate pad electrode are electrically shorted or a negative bias is applied to the gate pad electrode with respect to the source electrode; (d) passing a forward current through the built-in diode after the steps (b) and (c); (e) measuring a second on-voltage of the semiconductor device after the step (d); and (f) measuring a second on-voltage of the semiconductor device after the step (c). (g) after the step (f), for the semiconductor device selected as a conforming product, a step of measuring a second leakage current when a predetermined voltage is applied between the source electrode and the drain electrode in a state in which the source electrode and the gate pad electrode are electrically shorted or a negative bias is applied to the gate pad electrode with respect to the source electrode; and (h) after the step (g), a step of calculating a change between the second leakage current and the first leakage current, and if the change is smaller than a third specified value, selecting the semiconductor device as a conforming product. Effect of the Invention
[0019] According to one embodiment, the time required for screening the semiconductor device can be reduced, and the accuracy of sorting the semiconductor device can be made constant regardless of the product specifications. In addition, an electrical inspection device capable of achieving these can be provided. In addition, precise screening of the semiconductor device 100 can be performed, and a highly reliable semiconductor device 100 can be provided. [Brief description of the drawings]
[0020] [Figure 1] 1 is a cross-sectional view showing a semiconductor device in a first embodiment. [Diagram 2]2A to 2C are cross-sectional views showing a method for manufacturing the semiconductor device in FIG. [Diagram 3] 3 is a cross-sectional view showing the method of manufacturing the semiconductor device subsequent to FIG. 2. [Figure 4] 4 is a cross-sectional view showing the method of manufacturing the semiconductor device subsequent to FIG. 3. [Diagram 5] 1 is a cross-sectional view showing an electrical inspection device in accordance with a first embodiment. [Figure 6] 13 is a flowchart showing a current application method in the study example. [Figure 7] 1 is a graph showing the dependency of forward voltage on junction temperature (α curve). [Figure 8] 1 is a graph showing the behavior of the intersection of an α curve with Equation 1. [Figure 9] 1 is a graph showing the behavior of the intersection of an α curve with Equation 1. [Figure 10] 1 is a graph showing the behavior of the intersection of an α curve with Equation 1. [Figure 11] 4 is a flowchart showing a current application method (a method for manufacturing a semiconductor device) in the first embodiment. [Figure 12] 13 is a flowchart showing a preliminary experiment in the second embodiment. [Figure 13] 13 is a flowchart showing a current application method (a method for manufacturing a semiconductor device) in the second embodiment. [Figure 14] 11 is a graph showing the relationship between a change value ΔVon and a cumulative current application time. [Figure 15] 1 is a graph showing the relationship between leakage current Idss and cumulative current application time. [Figure 16] 13 is a flowchart showing a preliminary experiment in the third embodiment. [Figure 17] 13 is a flowchart showing a current application method (a method for manufacturing a semiconductor device) in the third embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] Hereinafter, the embodiments will be described in detail with reference to the drawings. In all the drawings for explaining the embodiments, the same reference numerals are used for the members having the same functions, and the repeated explanations are omitted. In the following embodiments, the explanations of the same or similar parts will not be repeated as a rule unless it is particularly necessary.
[0022] (Embodiment 1) The semiconductor device (semiconductor chip) 100, the electrical conductivity inspection device 200, and the electrical conductivity inspection method (semiconductor device manufacturing method) using the electrical conductivity inspection device 200 in the first embodiment will be described in order below.
[0023] <Semiconductor device> First, a semiconductor device 100 in the first embodiment will be described with reference to FIG. 1. Here, the semiconductor device 100 is illustrated as having an n-type SiC power MISFET, but the SiC power MISFET may be a p-type. In that case, the conductivity types of the impurities described below are all reversed. The SiC power MISFET has a vertical planar structure.
[0024] The semiconductor substrate 1 used in the first embodiment is a compound semiconductor substrate containing carbon and silicon, and is made of silicon carbide (SiC). The semiconductor substrate 1 has n-type conductivity, and has a front surface and a back surface opposite to the front surface.
[0025] A drain electrode 10 is formed on the back surface of the semiconductor substrate 1. The drain electrode 10 is, for example, a laminated film of a titanium film, a nickel film, and a gold film, and the thickness of the drain electrode 10 is, for example, 0.5 to 1.0 μm. The drain electrode 10 does not have to be a laminated film of these films, but may be a single layer film made of one of these films, or may be a conductive film other than these films.
[0026] An n-type semiconductor layer (epitaxial layer) 2 made of silicon carbide and having a lower impurity concentration than the semiconductor substrate 1 is formed on the surface of the semiconductor substrate 1. The semiconductor layer 2 functions as a drift layer and is electrically connected to the drain electrode 10. Therefore, a drain voltage is applied to the semiconductor layer 2 and the semiconductor substrate 1 from the drain electrode 10.
[0027] A p-type body region (impurity region) 3 is formed in the semiconductor layer 2. An n-type source region (impurity region) 4 is formed in the body region 3. The source region 4 has a higher impurity concentration than the semiconductor layer 2.
[0028] A gate electrode 6 is formed on the body region 3 and the semiconductor layer 2 via a gate insulating film 5. The gate insulating film 5 is an insulating film made of, for example, silicon oxide, and the gate electrode 6 is a conductive film such as polycrystalline silicon doped with n-type impurities. A gate voltage is applied to the gate electrode 6 from a gate pad electrode 9 described later.
[0029] The gate electrode 6 is covered with an interlayer insulating film 7. The interlayer insulating film 7 is an insulating film made of, for example, silicon oxide. The interlayer insulating film 7 has openings that expose part of the source region 4 and part of the body region 3.
[0030] A source electrode (source pad electrode) 8 is formed on the interlayer insulating film 7 so as to fill the opening of the interlayer insulating film 7 and to be electrically connected to the body region 3 and the source region 4. The source electrode 8 includes a barrier metal film and a conductive film formed on the barrier metal film. The barrier metal film is a laminated film including, for example, a titanium film and a titanium nitride film, and the conductive film is, for example, an aluminum film.
[0031] Although not shown here, an opening that exposes a part of the gate electrode 6 is also formed in the interlayer insulating film 7. A gate pad electrode 9 that is electrically connected to the gate electrode 6 is formed on the interlayer insulating film 7 so as to fill this opening. The gate pad electrode 9 is made of the same material as the source electrode 8.
[0032] Below, parameters such as the depth and impurity concentration of each component in the first embodiment are described. Note that each depth shown below is the depth from the surface of the semiconductor layer 2. In other words, these depths are the thicknesses of each impurity region.
[0033] The n-type semiconductor substrate 1 is, for example, 1×10 18 ~1×10 21 cm -3 The impurity concentration is
[0034] The n-type semiconductor layer 2 has a thickness of, for example, 5 to 50 μm and a thickness of, for example, 1×10 14 ~1×10 17 cm -3 The impurity concentration is
[0035] The p-type body region 3 has a depth of, for example, 500 to 2000 nm and a thickness of, for example, 1×10 16 ~1×10 19 cm -3 The impurity concentration is
[0036] The n-type source region 4 has a depth of, for example, 100 to 1000 nm and a thickness of, for example, 1×10 19 ~1×10 21 cm -3 The impurity concentration is
[0037] The gate electrode 6 functions as the gate of the SiC power MISFET, the source region 4 functions as the source of the SiC power MISFET, the semiconductor layer 2 functions as the drain of the SiC power MISFET, and the body region 3 located below the gate electrode 6 functions as the channel region of the SiC power MISFET. In addition, a parasitic pn diode formed by the p-type body region 3 and the n-type semiconductor layer 2 can be used as a built-in diode, and this built-in diode can be used as a freewheeling diode for use in an inverter.
[0038] <Method of manufacturing semiconductor device (SiC power MISFET)> A method for manufacturing the semiconductor device 100 will be described below with reference to FIGS.
[0039] First, a semiconductor substrate 1 is prepared as shown in Fig. 2. Next, a semiconductor layer 2 is formed on the surface of the semiconductor substrate 1 by, for example, epitaxial growth.
[0040] 3, a body region 3 is formed in the semiconductor layer 2 by photolithography and ion implantation. A source region 4 is then formed in the body region 3 by photolithography and ion implantation.
[0041] 4, a gate insulating film 5 is formed on the semiconductor layer 2 including the body region 3 and the source region 4, for example, by a chemical vapor deposition (CVD) method. Next, a gate electrode 6 is formed on the gate insulating film 5, for example, by a CVD method. Next, the gate electrode 6 is patterned by photolithography and etching.
[0042] Next, the interlayer insulating film 7 is formed on the semiconductor layer 2 by, for example, a CVD method so as to cover the gate electrode 6. Next, a part of the interlayer insulating film 7 is patterned by photolithography and etching to form a plurality of openings penetrating the interlayer insulating film 7 and the gate insulating film 5. The plurality of openings include an opening that reaches a part of the body region 3 and a part of the source region 4, and an opening that reaches a part of the gate electrode 6.
[0043] After the process of FIG. 4, the semiconductor device 100 shown in FIG. 1 is manufactured through the following process. First, a barrier metal film and a conductive film are sequentially formed on the interlayer insulating film 7 by, for example, a sputtering method or a CVD method so as to fill the openings in the interlayer insulating film 7. Next, the barrier metal film and the conductive film are patterned by a photolithography technique and an etching process to form a source electrode 8 and a gate pad electrode 9. The source electrode 8 is electrically connected to the body region 3 and the source region 4, and the gate pad electrode 9 is electrically connected to the gate electrode 6. Next, a drain electrode 10 is formed on the back surface of the semiconductor substrate 1 by, for example, a sputtering method or a CVD method. The drain electrode 10 is electrically connected to the semiconductor substrate 1 and the semiconductor layer 2.
[0044] Although detailed description is omitted here, a plurality of semiconductor devices 100 are manufactured on the semiconductor substrate 1 in a wafer state. The semiconductor substrate 1 in a wafer state is diced into individual pieces, whereby the semiconductor device 100 is obtained as a single semiconductor chip.
[0045] <Electrical inspection device> The electrical inspection device 200 according to the first embodiment will be described below with reference to FIG.
[0046] As shown in FIG. 5, the electrical conductivity inspection device 200 includes a cooling plate 21, an insulating plate 22, a control device 23, a measuring electrode 24, a conductive sheet 25, a measuring electrode 26, a measuring electrode 27, and a pressure vessel 28.
[0047] The cooling plate 21 is made of, for example, a copper plate having a nickel-plated surface. The cooling plate 21 has a cooling mechanism for cooling the heat generated from the semiconductor device 100 when the semiconductor device 100 is energized using the electrical conductivity inspection device 200.
[0048] The insulating plate 22 is provided on the cooling plate 21 and is made of, for example, ceramic or aluminum oxide. The insulating plate 22 also has therein a variable thermal resistance mechanism connected to the control device 23. The variable thermal resistance mechanism is, for example, a heat pump, a micro heat pump, or a heat pipe.
[0049] For example, the thermal resistance value of insulating plate 22 can be changed by using control device 23 to adjust the current flowing to the variable thermal resistance mechanism or adjust the gas flow rate flowing to the variable thermal resistance mechanism.
[0050] The measuring electrode 24 is provided on the insulating plate 22 and is made of, for example, a copper plate whose surface is gold-plated. The conductive sheet 25 is provided on the measuring electrode 24 and is made of, for example, graphite. The main function of the conductive sheet 25 is to promote thermal contact between the drain electrode 10 and the measuring electrode 24, and to equalize the temperature of the entire semiconductor device 100 by the high thermal conductivity within the surface of the conductive sheet 25. When a current is applied to the semiconductor device 100, the measuring electrode 24 is electrically connected to the drain electrode 10 via the conductive sheet 25, and a drain voltage is applied from the measuring electrode 24 to the drain electrode 10.
[0051] The measurement electrode 26 and the measurement electrode 27 are attached to a pressure vessel 28, provided above the measurement electrode 24, and positioned away from the measurement electrode 24. The semiconductor device 100 can be placed between the measurement electrode 24 and the measurement electrode 26, and between the measurement electrode 24 and the measurement electrode 27. When a current is applied to the semiconductor device 100, the measurement electrode 26 is electrically connected to the source electrode 8, a source voltage is applied from the measurement electrode 26 to the source electrode 8, the measurement electrode 27 is electrically connected to the gate pad electrode 9, and a gate voltage is applied from the measurement electrode 27 to the gate pad electrode 9.
[0052] The measuring electrodes 26 and 27 are needle-shaped and made of, for example, an alloy mainly composed of palladium, and other than palladium, may contain silver, gold, platinum, copper, etc. Also, while two measuring electrodes 26 and one measuring electrode 27 are illustrated in Fig. 5, the electrical conductivity inspection device 200 may be provided with a plurality of measuring electrodes 26 and a plurality of measuring electrodes 27.
[0053] The pressure vessel 28 is provided on the measurement electrode 24, and can change the internal pressure thereof to a pressure different from the external pressure thereof. When the semiconductor device 100 is installed between the measurement electrode 24 and the measurement electrode 26, and between the measurement electrode 24 and the measurement electrode 27, the semiconductor device 100 is accommodated inside the pressure vessel 28.
[0054] For example, when current is applied to the semiconductor device 100, the pressure inside the pressure vessel 28 can be set to a pressure higher than the pressure (atmospheric pressure) outside the pressure vessel 28. Moreover, the pressure vessel 28 is preferably made of an insulator such as glass or resin in order to prevent discharge when current is applied to the semiconductor device 100.
[0055] <Current application method in the study example> The current application method of the example studied by the present inventors will be described below with reference to FIG.
[0056] In the study example, similarly to Patent Document 1, the semiconductor device 100 is screened for suitability by calculating the change in on-voltage before and after passing a forward current through the built-in diode. For example, the semiconductor device 100 in which the change in on-voltage has increased due to the growth of stacking faults is screened as an unsuitable product.
[0057] Here, the inventors have found through their research that the growth of stacking faults causes a phenomenon in which the blocking breakdown voltage of the SiC power MISFET decreases. Furthermore, the inventors have also found through their research that this phenomenon occurs regardless of the change in the on-state voltage.
[0058] Therefore, in the current application method of the study example, the determination is made not only based on the change in the on-voltage but also based on the fluctuation in the blocking withstand voltage. The fluctuation in the blocking withstand voltage described here is determined based on the fluctuation in the leakage current Idss when a specified voltage is applied between the source electrode 8 and the drain electrode 10 in a state in which the source electrode 8 and the gate pad electrode 9 are electrically shorted, or in a state in which a negative bias is applied to the gate pad electrode with respect to the source electrode. To repeat, the current application method of the study example is not a conventionally known technology, but a new current application method devised by the present inventors.
[0059] The electrical inspection device used in the study example differs from electrical inspection device 200 in the first embodiment in that insulating plate 22 does not include a variable thermal resistance mechanism and pressure vessel 28 is not used.
[0060] First, in step S101, the semiconductor device 100 is prepared. That is, the semiconductor device 100 manufactured by the manufacturing process described with reference to FIGS. 1 to 4 is prepared. Next, the semiconductor device 100 is transferred to an electrical conductivity inspection device 200, and the semiconductor device 100 is placed between the measurement electrodes 24 and 26, and between the measurement electrodes 24 and 27. Then, the measurement electrode 24 is electrically connected to the drain electrode 10, the measurement electrode 26 is electrically connected to the source electrode 8, and the measurement electrode 27 is electrically connected to the gate pad electrode 9.
[0061] In step S102, with the source electrode 8 and the gate pad electrode 9 electrically shorted or with a negative bias applied to the gate pad electrode 9 relative to the source electrode 8, 0 V is applied to the source electrode 8 and a specified high voltage is applied to the drain electrode 10, and the leakage current Idss1 is measured.
[0062] In step S103, the junction temperature Tj of the semiconductor device 100 is set. The junction temperature Tj is set by passing a forward current If through the built-in diode. The forward current If is a current that flows from the source electrode 8 to the drain electrode 10 when a positive voltage is applied to the source electrode 8 and 0 V is applied to the drain electrode 10 in a state where the source electrode 8 and the gate pad electrode 9 are shorted, or in a state where a negative bias is applied to the gate pad electrode 9 with respect to the source electrode 8. Here, the forward current If is passed until the junction temperature Tj reaches 175° C., and the forward voltage Vf at that time is measured. The forward current If may be applied as a direct current or a pulse with an appropriate duty ratio, for example, 50%.
[0063] In step S104, the on-voltage Von1 in the initial state is measured. The on-voltage is the potential difference between the drain electrode 10 and the source electrode 8 when the SiC power MISFET is in the on-state. In other words, the on-voltage is the potential difference between the drain electrode 10 and the source electrode 8 when a positive voltage is applied to the drain electrode 10, 0 V is applied to the source electrode 8, and the voltage of the gate electrode 6 is gradually increased so that a current flows from the drain electrode 10 to the source electrode 8.
[0064] In step S105, stacking faults are grown by passing a forward current If through the built-in diode of the semiconductor device 100. Note that the conditions for applying the forward current If are the same as those in step S103.
[0065] In step S106, the on-voltage Von2 in the final state is measured in the same manner as in step S104.
[0066] In step S107, a change value ΔVon between the on-voltage Von2 and the on-voltage Von1 is calculated. The change value ΔVon is calculated by ΔVon=(Von2-Von1) / Von1. Note that the change value ΔVon described here is an absolute value.
[0067] In step S108, the change value ΔVon is determined. A change in on-voltage means that stacking faults have grown and the on-resistance has increased. If the change value ΔVon is smaller than a specified value, the semiconductor device 100 is selected as a conforming product. For example, if the change value ΔVon is less than 0.02 (YES), the semiconductor device 100 is selected as a conforming product. Then, the next step is step S109. If the change value ΔVon is 0.02 or more (NO), the semiconductor device 100 is selected as a non-conforming product, as in step S110.
[0068] In step S109, the leakage current Idss2 in the final state is measured in the same manner as in step S102.
[0069] In step S111, a change value ΔIdss between the leakage current Idss2 and the leakage current Idss1 is calculated. The change value ΔIdss is calculated by ΔIdss=Idss2-Idss1. Note that the change value ΔIdss described here is an absolute value.
[0070] In step S112, the change value ΔIdss is determined. If the change value ΔIdss is smaller than a specified value, the semiconductor device 100 is selected as a conforming product. For example, if the change value ΔIdss is less than 1 μA (YES), the semiconductor device 100 is selected as a conforming product. Then, the next step is step S113, where post-processing is performed on the semiconductor device 100. If the change value ΔIdss is 1 μA or more (NO), the semiconductor device 100 is selected as a non-conforming product as in step S114.
[0071] <Problems with the study example> The problems in the study example will be explained below with reference to FIGS.
[0072] In the examined example, when a forward current If is applied to the built-in diode, the maximum rated junction temperature Tjmax becomes a limiting factor, and there is a problem that it is difficult to make the forward current If equal to the maximum rated forward current Ifmax. If the forward current If cannot be made equal to the maximum rated forward current Ifmax, the current application time must be extended to grow stacking faults, which increases the time required for screening the semiconductor device. In order to make the forward current Ifmax equal, there is a method of pulse driving at an appropriate duty ratio to make the maximum rated junction temperature Tjmax, but in this case too, the current application time is extended by the reciprocal of the duty ratio, and therefore this is not an effective method.
[0073] 7 shows the dependency (α curve) of the forward voltage Vf on the junction temperature Tj of the semiconductor device 100 when the forward current If is in the range of 30 A to 50 A. The junction temperature Tj of the semiconductor device 100 in an equilibrium state due to thermal contact with the cooling plate 21 or the like is expressed by the following "Equation 1" using the thermal resistance value Rth. Note that Tcp is room temperature (25°C).
[0074] Tj=Tcp+Rth×Vf×If (Formula 1)
[0075] Here, as shown in Figure 8, "Equation 1" can be derived as a straight line of a linear function. For example, when the maximum rated junction temperature Tjmax is 175°C, if the thermal resistance value Rth is 0.7k / W, the intersection of the α curve at the maximum rated forward current Ifmax (50A) and Equation 1 can be calculated as the optimal condition.
[0076] On the other hand, as shown in FIG. 9, when the thermal resistance value Rth is 1.1 k / W, the junction temperature Tj at the intersection of the α curve and equation 1 becomes too high and exceeds 175° C., which is the maximum rated junction temperature Tjmax.
[0077] 10, even if the thermal resistance value Rth is 1.1 k / W, if the forward current If is set to about 35 A, the intersection point between the α curve and Equation 1 approaches the optimal condition. However, since the forward current If is low in FIG 10, the current flow time needs to be extended to grow stacking faults, and the time required for screening the semiconductor device 100 increases.
[0078] The growth rate of stacking faults is mainly determined by the concentration of holes accumulated inside the semiconductor layer 2 while the built-in diode is conducting, but the concentration of holes accumulated is largely dependent on the junction temperature Tj and the forward current If. Therefore, even in the case of FIG. 8, if the product specifications change, the maximum rated junction temperature Tjmax and the maximum rated forward current Ifmax will differ, and the conditions for growing stacking faults will change. In other words, if the thermal resistance value Rth is fixed, it is difficult to maintain a constant accuracy in selecting the semiconductor device 100.
[0079] Furthermore, the measurement of the leakage current Idss performed in steps S102 and S109 in the study example requires application of a voltage of several thousand volts, which cannot be performed with a normal electrical test device, and therefore steps S102 and S109 must be performed with a different device. Therefore, the time required for screening the semiconductor device 100 increases by the time required for the measurement by transferring the device to another device.
[0080] Furthermore, when measuring the leakage current Idss, a voltage of several thousand volts is applied, which makes it easy for discharge to occur. Therefore, the leakage current Idss may be measured at a voltage lower than the maximum rated voltage Vdss. In that case, the leakage current Idss1, the leakage current Idss2, and the change value ΔIdss are measured at a voltage lower than that in the case of the maximum rated voltage Vdss. Therefore, there is a risk that a breakdown voltage defect will occur in the semiconductor device 100 after post-processing or after production.
[0081] As described above, in consideration of the problems in the study example, a method is required that can reduce the time required for screening the semiconductor device 100 and can stabilize the accuracy of sorting the semiconductor device 100 regardless of the product specifications. Furthermore, if the leakage current Idss can be measured in addition to the on-voltage Von using the same electrical test device, the time required for screening the semiconductor device 100 can be further reduced.
[0082] <Current application method in the first embodiment (semiconductor device manufacturing method)> The energization method in the first embodiment will be described below with reference to Fig. 11. Note that steps S2 to S14 shown in Fig. 11 are performed on semiconductor device 100 between step S1 (the manufacturing process described with reference to Figs. 1 to 4) and the process subsequent to step S15, and therefore these steps can be collectively regarded as a "manufacturing method for a semiconductor device." In other words, the manufacturing method for a semiconductor device in the first embodiment includes the energization method of steps S2 to S14.
[0083] First, in step S1, the semiconductor device 100 is prepared. That is, the semiconductor device 100 is prepared by the manufacturing process described with reference to Figs. 1 to 4. Next, the semiconductor device 100 is transferred to an electrical conductivity inspection device 200, and the semiconductor device 100 is placed between the measurement electrodes 24 and 26, and between the measurement electrodes 24 and 27. Then, the measurement electrode 24 is electrically connected to the drain electrode 10, the measurement electrode 26 is electrically connected to the source electrode 8, and the measurement electrode 27 is electrically connected to the gate pad electrode 9.
[0084] In step S2, a junction temperature Tj of the semiconductor device 100 is set. The junction temperature Tj is set by passing a maximum rated forward current Ifmax through the built-in diode as a direct current. In addition, the maximum rated forward voltage Vfmax at that time is measured.
[0085] In step S3, it is determined whether the junction temperature Tj is the maximum rated junction temperature Tjmax. If the junction temperature Tj is the maximum rated junction temperature Tjmax (YES), the next step is step S4. If the junction temperature Tj is not the maximum rated junction temperature Tjmax (NO), in step S5, the resistance value of the variable thermal resistance mechanism of the insulating plate 22 is adjusted to adjust the thermal resistance value Rth in the above-mentioned "Equation 1." That is, the resistance value of the variable thermal resistance mechanism is adjusted so that the maximum rated junction temperature Tjmax is reached when the maximum rated forward current Ifmax is passed through the built-in diode. Steps S2, S3, and S5 are repeated until this state is reached.
[0086] In step S4, the on-voltage Von1 in the initial state is measured in the same manner as in step S104.
[0087] In step S6, the leakage current Idss1 in the initial state is measured. For example, in a state where the source electrode 8 and the gate pad electrode 9 are electrically shorted or a negative bias is applied to the gate pad electrode 9 with respect to the source electrode 8, 0V is applied to the source electrode 8, and a specified voltage is applied to the drain electrode 10, and the leakage current Idss1 is measured. Here, the specified voltage is the maximum rated voltage Vdss. Also, in step S6, the pressure inside the pressure vessel 28 is set to a pressure higher than the pressure outside the pressure vessel 28. This makes it possible to prevent discharge from occurring inside the pressure vessel 28 even if the maximum rated voltage Vdss, which is several thousand V, is applied.
[0088] In step S7, a forward current If is passed through the built-in diode of the semiconductor device 100 to grow stacking faults. Here, the forward current If is the maximum rated forward current Ifmax. That is, the maximum rated forward current Ifmax is passed through the built-in diode at the maximum rated junction temperature Tjmax.
[0089] In step S8, the on-voltage Von2 in the final state is measured in the same manner as in step S4.
[0090] In step S9, a change value ΔVon between the on-voltage Von2 and the on-voltage Von1 is calculated. The change value ΔVon is calculated by ΔVon=(Von2-Von1) / Von1. Note that the change value ΔVon described here is an absolute value.
[0091] In step S10, the change value ΔVon is determined. If the change value ΔVon is smaller than a specified value, it can be determined that there is no or almost no growth of stacking faults, and the semiconductor device 100 is selected as a conforming product. For example, if the change value ΔVon is less than 0.02 (YES), the semiconductor device 100 is selected as a conforming product. Then, the next step is step S11. If the change value ΔVon is 0.02 or more (NO), the semiconductor device 100 is selected as a non-conforming product, as in step S12.
[0092] In step S11, the leakage current Idss2 in the final state is measured in the same manner as in step S6.
[0093] In step S13, a change value ΔIdss between the leakage current Idss2 and the leakage current Idss1 is calculated. The change value ΔIdss is calculated by ΔIdss=Idss2-Idss1. Note that the change value ΔIdss described here is an absolute value.
[0094] In step S14, the change value ΔIdss is determined. If the change value ΔIdss is smaller than a specified value, it can be determined that there is no or almost no growth of stacking faults, and the semiconductor device 100 is selected as a conforming product. For example, if the change value ΔIdss is less than 1 μA (YES), the semiconductor device 100 is selected as a conforming product. Then, the next step is step S15, where post-processing is performed on the semiconductor device 100. If the change value ΔIdss is 1 μA or more (NO), the semiconductor device 100 is selected as a non-conforming product as in step S16.
[0095] In a normal electrical inspection device, the thermal resistance value Rth is fixed as in the study example. In contrast, in the electrical inspection device 200 of the first embodiment, the insulating plate 22 has a variable thermal resistance mechanism, so that the thermal resistance value Rth can be made variable. Therefore, the maximum rated forward current Ifmax can be passed through the built-in diode at the maximum rated junction temperature Tjmax. Therefore, the current passing time for growing stacking faults can be significantly shortened, and the time required for screening the semiconductor device 100 can be reduced.
[0096] In addition, since the thermal resistance value Rth can be made variable, the time required for screening the semiconductor device 100 can be minimized even if the product specifications change and the conditions for growing stacking faults change. In addition, when the maximum rated voltage Vdss of the product is low (e.g., 600V or 1200V), the ΔVon generally tends to be smaller than the high breakdown voltage (e.g., 3.3kV). This is because the thickness of the epitaxial layer constituting the semiconductor layer 2 becomes thinner. In such a case, the criteria for the on-state voltage may be relaxed or eliminated, and only the judgment of ΔIdss may be performed.
[0097] Furthermore, since the leakage current Idss can be measured at the maximum rated voltage Vdss, the risk of a breakdown voltage defect occurring in the semiconductor device 100 after post-processing can be reduced.
[0098] In addition to measuring the on-voltage Von, the leakage current Idss can also be measured by the same electrical testing device 200, which further reduces the time required for screening the semiconductor device 100 and enables precise screening of the semiconductor device 100. This makes it possible to provide a highly reliable semiconductor device 100.
[0099] (Embodiment 2) A current application method (a method for manufacturing a semiconductor device) in the second embodiment will be described below with reference to Figures 12 and 13. In the following description, differences from the first embodiment will be mainly described, and descriptions of points that overlap with the first embodiment will be omitted.
[0100] In the second embodiment, screening of the semiconductor device 100 is performed using a method different from that in the first embodiment. In the second embodiment, steps S40 to S49 shown in Fig. 13 are performed instead of steps S2 to S14 in the first embodiment shown in Fig. 11. That is, the method for manufacturing a semiconductor device in the second embodiment has a current application method of steps S40 to S49.
[0101] <Preliminary experiment> Before steps S40 to S49 shown in FIG. 13 are performed, the experiment shown in FIG. 12 is performed on each of a plurality of experimental semiconductor devices 100.
[0102] First, in step S20, a junction temperature Tj is set for the semiconductor device 100. The junction temperature Tj is set by passing a forward current If as a direct current through the built-in diode.
[0103] In step S21, it is determined whether the junction temperature Tj is the maximum rated junction temperature Tjmax. If the junction temperature Tj is the maximum rated junction temperature Tjmax (YES), the next step is step S22. If the junction temperature Tj is not the maximum rated junction temperature Tjmax (NO), in step S23, the forward current If passed through the built-in diode is adjusted until it reaches the maximum rated junction temperature Tjmax. In steps S22 and after, the adjusted forward current If and forward voltage Vf are used.
[0104] In step S24, the on-voltage Von1 in the initial state is measured. The method for measuring the on-voltage Von1 is the same as in step S4. In step S25, a forward current If is passed through the built-in diode of the semiconductor device 100 to grow stacking faults. In step S26, the on-voltage Von2 in the final state is measured in the same manner as in step S24. In step S27, the change value ΔVon between the on-voltage Von2 and the on-voltage Von1 is calculated. The change value ΔVon is calculated by ΔVon=(Von2-Von1) / Von1.
[0105] In step S28, it is determined whether or not ΔVon is saturated. If ΔVon is saturated, the next step is step S29. If ΔVon is not saturated, the process returns to step S25.
[0106] In step S29, it is determined whether or not sufficient sample data for the experiment has been acquired. Here, if the number of experimental semiconductor devices 100 is, for example, 100 or more, it is determined that the experimental data is sufficient, and the next step is step S30. If the number is less than 100, the process returns to step S24, and an experiment is performed on the next experimental semiconductor device 100. Note that the number of experimental semiconductor devices 100 is not limited to 100, and the more the better.
[0107] In step S30, the saturation time Tsat and the saturation change value ΔVonsat of the on-state voltage are determined. Fig. 14 is a graph showing the relationship between the change value ΔVon and the cumulative current application time obtained by this experiment.
[0108] Most of the semiconductor devices 100 used in the experiment have a graph shown in the "saturated group." In the "saturated group," the change value ΔVon hardly changes with the passage of current over time, and the change value ΔVon saturates. That is, in the "saturated group," stacking faults hardly increase with the passage of current over time, and there is no increase in resistance components. Therefore, the semiconductor devices 100 in the "saturated group" can be determined to be conforming products.
[0109] On the other hand, some of the multiple experimental semiconductor devices 100 may include those that are in the graph shown in the "non-saturated group." In the "non-saturated group," the change value ΔVon varies with the passage of current. That is, in the "non-saturated group," stacking faults increase with the passage of current, and the resistance component increases, causing fluctuations in the on-voltage. Therefore, the semiconductor devices 100 in the "non-saturated group" can be determined to be non-conforming products.
[0110] From the graph in Fig. 14, the energization time at which the change value ΔVon of the semiconductor device 100 in the "saturation group" is deemed to be sufficiently saturated can be determined as the saturation time Tsat. The first specified value shown in Fig. 14 is the value when the change value ΔVon between the on-voltage Von2 and the on-voltage Von1 of the semiconductor device 100 in the "saturation group" is saturated during the saturation time Tsat in this experiment (the saturated change value ΔVonsat of the on-voltage).
[0111] 14 is set as the saturation change value ΔVonsat of the on-voltage of the semiconductor device 100 in the "saturation group" when the saturation time Tsat is set as the current flow time "10". To ensure the reliability of screening of the semiconductor device 100, a longer current flow time can more reliably eliminate the "non-saturation group".
[0112] On the other hand, if the screening time is shortened to improve the productivity of the semiconductor device 100, a short current-flow time such as current-flow time "5" is preferable. In that case, there is a risk that the semiconductor device 100 in the "non-saturation group" will also be included. However, even if the current-flow time is relatively short, as shown in FIG. 15 described later, if it is confirmed by experiment that the leakage current Idss changes rapidly up to the current-flow time "5", it is possible to exclude the semiconductor device 100 in the "non-saturation group" with the change value ΔVon as a non-conforming product by screening based on the leakage current Idss, even if the current-flow time is "5".
[0113] Considering these circumstances, it is preferable to set the saturation time Tsat to a time that allows the setting of a first specified value that does not include the "non-saturation group" in Fig. 14. However, in order to shorten the current flow time, the saturation time Tsat may be set to a time that may include part of the "non-saturation group" in Fig. 14 and is longer than the time at which a sudden change in the leakage current Idss occurs in Fig. 15.
[0114] 12, leakage current Idss is also measured for a plurality of experimental semiconductor devices 100. In this measurement, experimental semiconductor devices 100 different from the experimental semiconductor devices 100 used in steps S24 to S30 are used. Steps S31 to S35 relating to the measurement of leakage current Idss will be described below.
[0115] In step S31, a forward current If is passed through the built-in diode of the semiconductor device 100 to grow stacking faults.
[0116] In step S32, the leakage current Idss is measured. For example, in a state where the source electrode 8 and the gate pad electrode 9 are electrically shorted or a negative bias is applied to the gate pad electrode 9 with respect to the source electrode 8, 0 V is applied to the source electrode 8 and a predetermined voltage is applied to the drain electrode 10, and the leakage current Idss is measured. Here, the predetermined voltage is the maximum rated voltage Vdss.
[0117] In step S33, it is determined whether the current-carrying time of the built-in diode has reached a cumulative predetermined time. That is, if the current-carrying time of the built-in diode has reached a cumulative predetermined time (the saturation time Tsat or a time set longer than the saturation time Tsat), the next step is step S34. If the current-carrying time of the built-in diode has not reached the cumulative predetermined time, the process returns to step S31.
[0118] In step S34, it is determined whether or not sufficient sample data for the experiment has been acquired. Here, similar to step S29, the number of semiconductor devices 100 for the experiment is 100 or more, and the more the number, the more preferable it is.
[0119] In step S35, the maximum leakage current Idssmax is determined. Fig. 15 is a graph showing the relationship between the leakage current Idss and the cumulative current application time obtained from this experiment.
[0120] Although the increase in the leakage current Idss tends to saturate with the passage of current flow time, there are cases where the leakage current Idss suddenly increases in some of the multiple experimental semiconductor devices 100. The inventors of the present application have made it clear through their studies that such sudden increases in the leakage current Idss can occur not only in the "non-saturation group" of FIG. 14 but also in the "saturation group."
[0121] Stacking faults grow along the basal plane, and it is speculated that if there is a specific dislocation that crosses the PN junction formed in the semiconductor substrate, the leakage current Idss is likely to increase, which is believed to be the cause of the sudden increase in leakage current Idss mentioned above.
[0122] Therefore, in the second embodiment, not only is screening judgement performed using the first specified value, but screening judgement is also performed by setting a second specified value for the semiconductor device 100 in which a certain level of leakage current Idss occurs.
[0123] This second specified value is set with reference to the leakage current Idss measured in step S33. For example, the second specified value is set to the largest leakage current Idss value after excluding leakage currents with sudden increases in the leakage current Idss, or to a value slightly larger than the leakage current Idss. The second specified value thus set is the maximum leakage current Idssmax. At this time, it is confirmed whether leakage currents with sudden increases in the leakage current Idss can be excluded during the current application time of the saturation time Tsat. Therefore, the cumulative predetermined time in step S33 is set to a time equal to or greater than the saturation time Tsat.
[0124] As described above, by conducting the experiment of FIG. 12 in advance on multiple experimental semiconductor devices 100, the saturation time Tsat, the first specified value (saturation change value ΔVonsat of the on-voltage) and the second specified value (maximum leakage current Idssmax) are determined based on the results.
[0125] <Current application method in the second embodiment (semiconductor device manufacturing method)> The energization method (semiconductor device manufacturing method) of the second embodiment will be described below with reference to Fig. 13. The energization method (semiconductor device manufacturing method) of the second embodiment can be implemented without using the energization inspection device 200, but may be implemented using the energization inspection device 200 as in the first embodiment.
[0126] First, in step S40, a semiconductor device 100 is prepared. That is, similarly to the first embodiment, a semiconductor device 100 is prepared which is manufactured by the manufacturing process described with reference to FIGS.
[0127] In step S41, an on-state voltage Von1 is measured in the same manner as in step S24. In step S42, a forward current If is passed through the built-in diode of the semiconductor device 100 for a saturation time Tsat to grow stacking faults.
[0128] In step S43, it is confirmed whether the conduction time of the built-in diode has reached the saturation time Tsat. If the conduction time has reached the saturation time Tsat (YES), the next step is step S44. If the conduction time has not reached the saturation time Tsat (NO), step S42 is repeated until the conduction time reaches the saturation time Tsat. In step S44, the on-voltage Von2 in the final state is measured in the same manner as in step S41.
[0129] In step S45, a change value ΔVon between the on-voltage Von2 and the on-voltage Von1 is calculated by the equation ΔVon=(Von2−Von1) / Von1.
[0130] In step S46, the change value ΔVon is determined. If the change value ΔVon is smaller than the first specified value (saturation change value ΔVonsat of the on-state voltage) (YES), the semiconductor device 100 is selected as a conforming product. Then, the next step is step S47. If the change value ΔVon is larger than the first specified value (NO), the semiconductor device 100 is selected as a non-conforming product as in step S48.
[0131] In step S47, the leakage current Idss is measured in the same manner as in step S31. Note that the leakage current Idss is measured at the maximum rated voltage of the semiconductor device 100.
[0132] In step S49, the leakage current Idss is judged. If the leakage current Idss is smaller than the second specified value (maximum leakage current Idssmax) (YES), the semiconductor device 100 is selected as a conforming product. Then, the next step is step S50, where post-processing is performed on the semiconductor device 100. If the leakage current Idss is larger than the second specified value (NO), the semiconductor device 100 is selected as a non-conforming product as in step S51.
[0133] In this manner, in the second embodiment, the conduction time of the built-in diode is set as the saturation time Tsat, and the first specified value (saturation change value ΔVonsat of the on-voltage) and the second specified value (maximum leakage current Idssmax) are used, thereby enabling precise screening of the semiconductor device 100. Therefore, it is possible to select a semiconductor device 100 having a small change value ΔVon of the on-voltage and a small leakage current Idss, thereby making it possible to provide a highly reliable semiconductor device 100.
[0134] (Embodiment 3) A current application method (a method for manufacturing a semiconductor device) in the third embodiment will be described below with reference to Figures 16 and 17. In the following description, differences from the second embodiment will be mainly described, and descriptions of points that overlap with the second embodiment will be omitted.
[0135] In the second embodiment, the leakage current Idss is selected by comparing with the second specified value (maximum leakage current Idssmax). In the third embodiment, the leakage current Idss is selected using the change value ΔIdss as in the first embodiment. Therefore, in the third embodiment, a part of steps S40 to S49 in the second embodiment shown in FIG. 13 is replaced with steps S70 to S73 shown in FIG.
[0136] <Preliminary experiment> Before performing steps S40 to S48 and S70 to S73 shown in Fig. 17, the experiments shown in Fig. 16 are performed on a plurality of experimental semiconductor devices 100. Note that the experiments related to the first specified value (saturation change value ΔVonsat of the on-state voltage) are the same as steps S20 to S30 in the second embodiment, and therefore the description thereof will be omitted.
[0137] First, step S60 is performed after step S22. In step S60, the leakage current Idss1 is measured using the same method as in step S32. The leakage current Idss1 is measured at the maximum rated voltage of the semiconductor device 100. In step S61, a forward current If is passed through the built-in diode of the semiconductor device 100 to grow stacking faults. In step S62, the leakage current Idss2 is measured using the same method as in step S60. The leakage current Idss2 is measured at the maximum rated voltage of the semiconductor device 100.
[0138] In step S63, it is determined whether the current-carrying time of the built-in diode has reached a predetermined cumulative time. That is, if the current-carrying time of the built-in diode has reached a predetermined cumulative time (the saturation time Tsat or a time set longer than the saturation time Tsat), the next step is step S64. If the current-carrying time of the built-in diode has not reached the predetermined cumulative time, the process returns to step S61.
[0139] In step S64, it is determined whether or not sufficient sample data for the experiment has been acquired. Here, as in step S29, the number of semiconductor devices 100 for the experiment is 100 or more, and the more the number, the more preferable it is.
[0140] In step S65, a change in leakage current ΔIdss is calculated by the formula ΔIdss=Idss2−Idss1.
[0141] In step S66, the maximum change value ΔIdssmax of the leakage current is determined as the third specified value. This third specified value is set by referring to the change value ΔIdss calculated in step S64. For example, the third specified value is set to the maximum change value ΔIdss among the change values ΔIdss calculated for the multiple experimental semiconductor devices 100 after excluding those with sudden increases in the leakage current Idss shown in FIG. 15, or to a value slightly larger than the change value ΔIdss. The third specified value thus set is the maximum change value ΔIdssmax of the leakage current. The maximum change value ΔIdssmax is, for example, 1 μA.
[0142] As described above, by conducting the experiment of FIG. 16 in advance on multiple experimental semiconductor devices 100, the saturation time Tsat, the first specified value (saturation change value ΔVonsat of the on-voltage) and the third specified value (maximum change value ΔIdssmax of the leakage current) are determined based on the results of the experiment.
[0143] <Current application method in the third embodiment (semiconductor device manufacturing method)> The energization method (semiconductor device manufacturing method) of the third embodiment will be described below with reference to Fig. 17. The energization method (semiconductor device manufacturing method) of the third embodiment can be implemented without using the energization inspection device 200, but may be implemented using the energization inspection device 200 as in the first embodiment.
[0144] In the third embodiment, step S70 is performed between steps S41 and S42. Note that step S70 may be performed between steps S40 and S41. In step S70, the leakage current Idss1 is measured using the same method as in step S60. Thereafter, steps S42 to S48 are performed as in the second embodiment. Steps S71 to S73 are performed on the semiconductor device 100 selected as a suitable product in step S46.
[0145] In step S71, the leakage current Idss2 is measured using the same method as in step S62. The leakage current Idss2 is measured at the maximum rated voltage of the semiconductor device 100. In step S72, a change value ΔIdss in the leakage current is calculated. The change value ΔIdss is calculated by ΔIdss=Idss2-Idss1.
[0146] In step S73, the change value ΔIdss is judged. If the change value ΔIdss is smaller than a third specified value (the maximum change value ΔIdssmax of leakage current) (YES), the semiconductor device 100 is selected as a conforming product. Then, the next step is step S50, where post-processing is performed on the semiconductor device 100. If the change value ΔIdss is larger than the third specified value (NO), the semiconductor device 100 is selected as a non-conforming product as in step S51.
[0147] In this manner, in the third embodiment, the conduction time of the built-in diode is set as the saturation time Tsat, and the first specified value (saturation change value ΔVonsat of the on-voltage) and the third specified value (maximum change value ΔIdssmax of the leakage current) are used, thereby enabling precise screening of the semiconductor device 100. Therefore, it is possible to select a semiconductor device 100 having a small change value ΔVon of the on-voltage and a small leakage current Idss, thereby enabling the provision of a highly reliable semiconductor device 100.
[0148] Although the present invention has been specifically described above based on the above embodiment, the present invention is not limited to the above embodiment and can be modified in various ways without departing from the spirit of the present invention. [Explanation of symbols]
[0149] 1. Semiconductor substrate 2. Semiconductor layer 3. Body Region 4 Source Area 5 Gate insulating film 6 Gate electrode 7 Interlayer insulating film 8 Source electrode (source pad electrode) 9 Gate pad electrode 10 Drain electrode 21 Cooling plate 22 Insulating plate 23 Control Equipment 24 Measuring electrode 25 Conductive sheet 26 Measuring electrode 27 Measuring electrode 28 Pressure Vessels 100 Semiconductor devices (semiconductor chips) 200 Electrical inspection device
Claims
1. A cooling plate; an insulating plate provided on the cooling plate; A first electrode provided on the insulating plate; a second electrode and a third electrode disposed above the first electrode and spaced apart from the first electrode; Equipped with The insulating plate has a variable thermal resistance mechanism, A semiconductor device can be placed between the first electrode and the second electrode, and between the first electrode and the third electrode.
2. 2. The electrical inspection device according to claim 1, A pressure vessel is provided on the first electrode and the pressure therein can be changed to a pressure different from the pressure thereout, the second electrode and the third electrode are attached to the pressure vessel; An electrical conductivity inspection device, wherein when the semiconductor device is installed between the first electrode and the second electrode, and between the first electrode and the third electrode, the semiconductor device is contained inside the pressure vessel.
3. 3. The electrical inspection device according to claim 2, The pressure vessel is made of an insulator,
4. A cooling plate; an insulating plate provided on the cooling plate and having a variable thermal resistance mechanism; A first electrode provided on the insulating plate; a second electrode and a third electrode disposed above the first electrode and spaced apart from the first electrode; A method for manufacturing a semiconductor device using an electrical inspection device comprising: (a) providing a semiconductor device including a drain electrode, a source electrode, and a gate pad electrode; (b) after the step (a), placing the semiconductor device between the first electrode and the second electrode and between the first electrode and the third electrode, electrically connecting the first electrode to the drain electrode, electrically connecting the second electrode to the source electrode, and electrically connecting the third electrode to the gate pad electrode; (c) after the step (b), adjusting the resistance value of the variable thermal resistance mechanism so that the semiconductor device has a maximum rated junction temperature when a maximum rated forward current of the semiconductor device is applied to a built-in diode of the semiconductor device; (d) measuring a first on-voltage of the semiconductor device after the step (c); (e) after the step (c), measuring a first leakage current when a specified voltage is applied between the source electrode and the drain electrode in a state in which the source electrode and the gate pad electrode are electrically shorted or in a state in which a negative bias is applied to the gate pad electrode with respect to the source electrode; (f) after the steps (d) and (e), a step of passing a forward current through the built-in diode; (g) measuring a second on-voltage of the semiconductor device after the step (f); (h) after the step (g), calculating a change in the second on-voltage and the first on-voltage, and if the change is smaller than a specified value, selecting the semiconductor device as a conforming product; (i) after the step (h), for the semiconductor device selected as a conforming product, a step of measuring a second leakage current when a specified voltage is applied between the source electrode and the drain electrode in a state in which the source electrode and the gate pad electrode are electrically shorted or in a state in which a negative bias is applied to the gate pad electrode with respect to the source electrode; (j) after the step (i), calculating a change in the second leakage current and the first leakage current, and selecting the semiconductor device as a conforming product if the change in the second leakage current is smaller than a specified value; Equipped with The step (a) comprises: (a1) preparing a semiconductor substrate of a first conductivity type having a front surface and a back surface opposite to the front surface and made of silicon carbide; (a2) forming a semiconductor layer of the first conductivity type made of silicon carbide on the surface of the semiconductor substrate; (a3) forming a body region of a second conductivity type, opposite to the first conductivity type, in the semiconductor layer; (a4) forming a source region of the first conductivity type in the body region; (a5) forming a gate insulating film on the body region; (a6) forming a gate electrode on the gate insulating film; (a7) forming the source electrode on the body region and on the source region so as to be electrically connected to the body region and the source region, and forming the gate pad electrode on the gate electrode so as to be electrically connected to the gate electrode; (a8) forming the drain electrode on the back surface of the semiconductor substrate; Including, The built-in diode is configured by the body region and the semiconductor layer.
5. 5. The method of manufacturing a semiconductor device according to claim 4, In the step (f), a maximum rated forward current of the semiconductor device is passed through a built-in diode of the semiconductor device at a maximum rated junction temperature of the semiconductor device.
6. 6. The method for manufacturing a semiconductor device according to claim 5, A method for manufacturing a semiconductor device, wherein in the steps (e) and (i), the first leakage current and the second leakage current are measured at a maximum rated voltage of the semiconductor device.
7. 7. The method of manufacturing a semiconductor device according to claim 6, The electrical conductivity inspection device further includes a pressure vessel provided on the first electrode and capable of changing the internal pressure thereof to a pressure different from the external pressure thereof; the second electrode and the third electrode are attached to the pressure vessel; In the step (b), the semiconductor device is accommodated inside the pressure vessel; A method for manufacturing a semiconductor device, wherein in the steps (e) and (i), the pressure inside the pressure vessel is higher than the pressure outside the pressure vessel.
8. 8. The method of manufacturing a semiconductor device according to claim 7, The method for manufacturing a semiconductor device, wherein the pressure vessel is made of an insulator.
9. A cooling plate; an insulating plate provided on the cooling plate and having a variable thermal resistance mechanism; A first electrode provided on the insulating plate; a second electrode and a third electrode disposed above the first electrode and spaced apart from the first electrode; An energization method using an energization inspection device comprising: (a) providing a semiconductor device including a drain electrode, a source electrode, and a gate pad electrode; (b) after the step (a), placing the semiconductor device between the first electrode and the second electrode and between the first electrode and the third electrode, electrically connecting the first electrode to the drain electrode, electrically connecting the second electrode to the source electrode, and electrically connecting the third electrode to the gate pad electrode; (c) after the step (b), adjusting the resistance value of the variable thermal resistance mechanism so that the semiconductor device has a maximum rated junction temperature when a maximum rated forward current of the semiconductor device is applied to a built-in diode of the semiconductor device; (d) measuring a first on-voltage of the semiconductor device after the step (c); (e) after the step (c), measuring a first leakage current when a specified voltage is applied between the source electrode and the drain electrode in a state in which the source electrode and the gate pad electrode are electrically shorted or in a state in which a negative bias is applied to the gate pad electrode with respect to the source electrode; (f) after the steps (d) and (e), a step of passing a forward current through the built-in diode; (g) measuring a second on-voltage of the semiconductor device after the step (f); (h) after the step (g), calculating a change in the second on-voltage and the first on-voltage, and if the change is smaller than a specified value, selecting the semiconductor device as a conforming product; (i) after the step (h), for the semiconductor device selected as a conforming product, a step of measuring a second leakage current when a specified voltage is applied between the source electrode and the drain electrode in a state in which the source electrode and the gate pad electrode are electrically shorted or in a state in which a negative bias is applied to the gate pad electrode with respect to the source electrode; (j) after the step (i), calculating a change in the second leakage current and the first leakage current, and selecting the semiconductor device as a conforming product if the change in the second leakage current is smaller than a specified value; Equipped with The semiconductor device includes: a semiconductor substrate of a first conductivity type having a front surface and a back surface opposite to the front surface and made of silicon carbide; a semiconductor layer of the first conductivity type formed on the surface of the semiconductor substrate and made of silicon carbide; a body region of a second conductivity type opposite to the first conductivity type formed in the semiconductor layer; a source region of the first conductivity type formed in the body region; a gate insulating film formed on the body region; a gate electrode formed on the gate insulating film; a source electrode formed on the body region and on the source region so as to be electrically connected to the body region and the source region; a gate pad electrode formed on the gate electrode so as to be electrically connected to the gate electrode; the drain electrode formed on the back surface of the semiconductor substrate; Including, The built-in diode is constituted by the body region and the semiconductor layer.
10. The current supply method according to claim 9, In the step (f), a maximum rated forward current of the semiconductor device is passed through a built-in diode of the semiconductor device at a maximum rated junction temperature of the semiconductor device.
11. The method according to claim 10, A current-passing method, wherein in the step (e) and the step (i), the first leakage current and the second leakage current are measured at a maximum rated voltage of the semiconductor device.
12. The method according to claim 11, The electrical conductivity inspection device further includes a pressure vessel provided on the first electrode and capable of changing the internal pressure thereof to a pressure different from the external pressure thereof; the second electrode and the third electrode are attached to the pressure vessel; In the step (b), the semiconductor device is accommodated inside the pressure vessel; A current application method, wherein in the step (e) and the step (i), the pressure inside the pressure vessel is higher than the pressure outside the pressure vessel.
13. The method according to claim 12, A method for applying electricity, wherein the pressure vessel is made of an insulator.
14. (a) preparing a semiconductor device including a drain electrode, a source electrode, a gate pad electrode and a built-in diode; (b) measuring a first on-voltage of the semiconductor device after the step (a); (c) after the step (b), a step of passing a forward current through the built-in diode; (d) measuring a second on-voltage of the semiconductor device after the step (c); (e) after the step (d), calculating a change in the second on-voltage and the first on-voltage, and selecting the semiconductor device as a conforming product if the change in the second on-voltage is smaller than a first specified value; (f) after the step (e), for the semiconductor device selected as a conforming product, a step of measuring a leakage current when a predetermined voltage is applied between the source electrode and the drain electrode in a state in which the source electrode and the gate pad electrode are electrically shorted or in a state in which a negative bias is applied to the gate pad electrode with respect to the source electrode; (g) after the step (f), if the leakage current is smaller than a second specified value, selecting the semiconductor device as a conforming product; Equipped with the first specified value and the second specified value are set based on results of experiments previously performed on a plurality of experimental semiconductor devices; The above experiments were carried out as follows: (x1) measuring a first on-voltage of the semiconductor device; (x2) after the step (x1), a step of passing a forward current through the built-in diode for a first saturation time; (x3) measuring a second on-voltage of the semiconductor device after the (x2) step; (x4) after the step (x3), calculating a change in the second on-voltage and the first on-voltage during an experiment; having the first specified value is a value at which a change value between the second on-state voltage and the first on-state voltage becomes saturated during the first saturation time in the experiment, The method for manufacturing a semiconductor device, wherein the step (c) is performed for a first saturation time.
15. 15. The method of manufacturing a semiconductor device according to claim 14, The above experiments were carried out as follows: (y1) flowing a forward current through the built-in diode for the first saturation time; (y2) after the step (y1), a step of measuring a leakage current when a predetermined voltage is applied between the source electrode and the drain electrode in a state in which the source electrode and the gate pad electrode are electrically shorted or in a state in which a negative bias is applied to the gate pad electrode with respect to the source electrode; and The method for manufacturing a semiconductor device, wherein the second specified value is set with reference to the leakage current measured in the (y2) step.
16. 16. The method of manufacturing a semiconductor device according to claim 15, The method for manufacturing a semiconductor device, wherein the leakage current in the step (f) and the leakage current in the step (y2) are measured at a maximum rated voltage of the semiconductor device.
17. 15. The method of manufacturing a semiconductor device according to claim 14, The step (a) comprises: (a1) preparing a semiconductor substrate of a first conductivity type having a front surface and a back surface opposite to the front surface and made of silicon carbide; (a2) forming a semiconductor layer of the first conductivity type made of silicon carbide on the surface of the semiconductor substrate; (a3) forming a body region of a second conductivity type, opposite to the first conductivity type, in the semiconductor layer; (a4) forming a source region of the first conductivity type in the body region; (a5) forming a gate insulating film on the body region; (a6) forming a gate electrode on the gate insulating film; (a7) forming the source electrode on the body region and on the source region so as to be electrically connected to the body region and the source region, and forming the gate pad electrode on the gate electrode so as to be electrically connected to the gate electrode; (a8) forming the drain electrode on the back surface of the semiconductor substrate; Including, The built-in diode is configured by the body region and the semiconductor layer.
18. (a) preparing a semiconductor device including a drain electrode, a source electrode, a gate pad electrode and a built-in diode; (b) measuring a first on-voltage of the semiconductor device after the step (a); (c) after the step (a), measuring a first leakage current when a specified voltage is applied between the source electrode and the drain electrode in a state in which the source electrode and the gate pad electrode are electrically shorted or in a state in which a negative bias is applied to the gate pad electrode with respect to the source electrode; (d) after the steps (b) and (c), a step of passing a forward current through the built-in diode; (e) measuring a second on-voltage of the semiconductor device after the step (d); (f) after the step (e), calculating a change in the second on-voltage and the first on-voltage, and selecting the semiconductor device as a conforming product if the change in the second on-voltage is smaller than a first specified value; (g) after the step (f), for the semiconductor device selected as a conforming product, a step of measuring a second leakage current when a predetermined voltage is applied between the source electrode and the drain electrode in a state in which the source electrode and the gate pad electrode are electrically shorted or in a state in which a negative bias is applied to the gate pad electrode with respect to the source electrode; (h) after the step (g), calculating a change in the second leakage current and the first leakage current, and selecting the semiconductor device as a conforming product if the change in the second leakage current is smaller than a third specified value; Equipped with the first specified value and the third specified value are set based on results of experiments previously performed on a plurality of experimental semiconductor devices; The above experiments were carried out as follows: (x1) measuring a first on-voltage of the semiconductor device; (x2) after the step (x1), a step of passing a forward current through the built-in diode for a first saturation time; (x3) measuring a second on-voltage of the semiconductor device after the (x2) step; (x4) after the step (x3), calculating a change in the second on-voltage and the first on-voltage during an experiment; having the first specified value is a value at which a change value between the second on-state voltage and the first on-state voltage becomes saturated during the first saturation time in the experiment, The method for manufacturing a semiconductor device, wherein the step (d) is performed for a first saturation time.
19. 20. The method of manufacturing a semiconductor device according to claim 18, The above experiments were carried out as follows: (z1) measuring a first leakage current when a specified voltage is applied between the source electrode and the drain electrode in a state in which the source electrode and the gate pad electrode are electrically shorted or in a state in which a negative bias is applied to the gate pad electrode with respect to the source electrode; (z2) after the step (z1), a step of passing a forward current through the built-in diode for the first saturation time; (z3) after the step (z2), a step of measuring a second leakage current when a predetermined voltage is applied between the source electrode and the drain electrode in a state in which the source electrode and the gate pad electrode are electrically shorted or in a state in which a negative bias is applied to the gate pad electrode with respect to the source electrode; (z4) after the step (z3), calculating a change in the second leakage current and the first leakage current; and The method for manufacturing a semiconductor device, wherein the third specified value is set by referring to the change value calculated in the (z4) step.
20. 20. The method of manufacturing a semiconductor device according to claim 19, A method for manufacturing a semiconductor device, wherein the first leakage current in the step (c), the second leakage current in the step (g), the first leakage current in the step (z1), and the second leakage current in the step (z3) are measured by a maximum rated voltage of the semiconductor device.
21. 20. The method of manufacturing a semiconductor device according to claim 18, The step (a) comprises: (a1) preparing a semiconductor substrate of a first conductivity type having a front surface and a back surface opposite to the front surface and made of silicon carbide; (a2) forming a semiconductor layer of the first conductivity type made of silicon carbide on the surface of the semiconductor substrate; (a3) forming a body region of a second conductivity type, opposite to the first conductivity type, in the semiconductor layer; (a4) forming a source region of the first conductivity type in the body region; (a5) forming a gate insulating film on the body region; (a6) forming a gate electrode on the gate insulating film; (a7) forming the source electrode on the body region and on the source region so as to be electrically connected to the body region and the source region, and forming the gate pad electrode on the gate electrode so as to be electrically connected to the gate electrode; (a8) forming the drain electrode on the back surface of the semiconductor substrate; Including, The built-in diode is configured by the body region and the semiconductor layer.
22. 22. The method of manufacturing a semiconductor device according to claim 21, The steps (b) to (h) are carried out using an electrical inspection device; The electrical conductivity inspection device includes: A cooling plate; an insulating plate provided on the cooling plate and having a variable thermal resistance mechanism; A first electrode provided on the insulating plate; a second electrode and a third electrode disposed above the first electrode and spaced apart from the first electrode; Equipped with After the step (a) and before the steps (b) and (c), (i) after the step (a), placing the semiconductor device between the first electrode and the second electrode and between the first electrode and the third electrode, electrically connecting the first electrode to the drain electrode, electrically connecting the second electrode to the source electrode, and electrically connecting the third electrode to the gate pad electrode; (j) after the step (i), adjusting the resistance value of the variable thermal resistance mechanism so that the maximum rated junction temperature of the semiconductor device is reached when a maximum rated forward current of the semiconductor device is passed through a built-in diode of the semiconductor device; A manufacturing method of a semiconductor device comprising:
23. 23. The method of manufacturing a semiconductor device according to claim 22, In the step (d), a maximum rated forward current of the semiconductor device is passed through a built-in diode of the semiconductor device at a maximum rated junction temperature of the semiconductor device.
24. 24. The method of manufacturing a semiconductor device according to claim 23, The method for manufacturing a semiconductor device, wherein the first leakage current in the step (c) and the second leakage current in the step (g) are measured at a maximum rated voltage of the semiconductor device.
25. 25. The method of manufacturing a semiconductor device according to claim 24, The electrical conductivity inspection device further includes a pressure vessel provided on the first electrode and capable of changing the internal pressure thereof to a pressure different from the external pressure thereof; the second electrode and the third electrode are attached to the pressure vessel; In the step (i), the semiconductor device is accommodated inside the pressure vessel, A method for manufacturing a semiconductor device, wherein in the steps (c) and (g), the pressure inside the pressure vessel is higher than the pressure outside the pressure vessel.
26. 26. The method of manufacturing a semiconductor device according to claim 25, The method for manufacturing a semiconductor device, wherein the pressure vessel is made of an insulator.
Citation Information
Patent Citations
Energization test device and energization test method
JP2017212317A
Method for selecting silicon carbide semiconductor device
JP2018205252A
Manufacturing method of silicon carbide semiconductor device and silicon carbide semiconductor inspection device
JP2019216202A
Selecting method of silicon carbide semiconductor device
JP2020150181A
Semiconductor device inspection method and inspection device
JP2020187102A