Polyamide Polymer

A polyamide-based polymer using itaconic acid and specific diamines addresses the environmental issues of nylon by providing water resistance, biodegradability, and mechanical strength, suitable for fishing gear and automotive applications.

JP7593612B2Active Publication Date: 2024-12-03GRIPS CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020168489
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-10-05
Publication Date
2024-12-03
Estimated Expiration
2040-10-05

AI Technical Summary

Technical Problem

Conventional nylon polymers exhibit poor water resistance and non-biodegradability, leading to environmental pollution and safety issues such as entanglement in marine life, while alternatives with comparable mechanical strength and durability are lacking.

Method used

A polyamide-based polymer is developed using itaconic acid and specific diamines, with controlled molar ratios, to achieve moderate water resistance, biodegradability, and mechanical strength comparable to nylon.

Benefits of technology

The polymer demonstrates appropriate water resistance, biodegradability, and mechanical strength, making it suitable as a sustainable alternative for nylon in applications like fishing gear and automotive parts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007593612000011
    Figure 0007593612000011
  • Figure 0007593612000012
    Figure 0007593612000012
  • Figure 0007593612000013
    Figure 0007593612000013
Patent Text Reader

Abstract

To provide a polyamide-based polymer which uses as the raw material an itaconic acid capable of being obtained as a bio basis monomer, has appropriate waterproofness, both resolvability and durability in water, and mechanical strength comparable to that of nylon, and can be a substitute for nylon.SOLUTION: A polyamide-based polymer obtained by polymerizing a dicarboxylic acid and a diamine is such that: as the dicarboxylic acid, an itaconic acid is used; and as the diamine, a diamine represented by formula (I): H2 N-R1-NH2 (I) (where R1 represents a 6-12C straight-chain alkylene group), and a diamine represented by formula (II): H2 N-R2-NH2 (II) (where R2 represents a 6-12C alkylene group having a 1-4C alkyl group as the branched chain) are used together.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polyamide-based polymer. More specifically, the present invention relates to a polyamide-based polymer that is expected to be used as a replacement for conventional nylon (trade name). [Background technology]

[0002] Polyamides, such as nylon (product name, hereinafter the same), are not only used as fibers, but also have excellent properties such as heat resistance and oil resistance, so they are widely used in parts around automobile engines, such as intake manifolds.

[0003] In recent years, polyamides obtained by reacting itaconic acid with an aliphatic dialkylenediamine having 2 to 6 methylene groups or an aromatic diamine such as diaminodiphenyl ether or xylylenediamine, followed by dehydration condensation, have been proposed as polyamides having a high glass transition temperature and performance as engineering plastics (see, for example, paragraph

[0016] and Examples of Patent Document 1). However, the polyamides have the drawback of being poor in water resistance because they dissolve in water in a short time when exposed to light in water.

[0004] Traditionally, fishing gear such as fishing nets and fishing lines used in the fishing industry are made of nylon, which has water resistance and high mechanical strength such as tensile strength. However, in today's world where marine pollution by plastic waste has become an international issue, plastic waste such as nylon is poorly degradable in nature and drifts in the ocean without decomposing, which has raised concerns that fish and other animals may mistakenly ingest plastic waste, and that nylon fishing lines may get tangled in the wings or legs of seabirds.

[0005] Therefore, there is an urgent need to develop a plastic that can replace nylon, which has both degradability in water and durability, and mechanical strength comparable to that of nylon. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Patent No. 5777134 Summary of the Invention [Problem to be solved by the invention]

[0007] The present invention has been made in view of the above-mentioned conventional techniques, and an object of the present invention is to provide a polyamide-based polymer which uses itaconic acid, which is available as a bio-based monomer, as a raw material, has appropriate water resistance, as well as degradability in water and durability, and has mechanical strength comparable to that of nylon, and which can serve as a substitute for nylon. [Means for solving the problem]

[0008] The present invention relates to (1) A polyamide-based polymer obtained by polymerizing a dicarboxylic acid and a diamine, wherein the dicarboxylic acid is itaconic acid and the diamine is a compound represented by the formula (I): H2N-R 1 -NH2(I) (In the formula, R 1 represents a straight-chain alkylene group having 6 to 12 carbon atoms. and a diamine represented by formula (II): H2N-R 2 -NH2(II) (In the formula, R 2 represents an alkylene group having 6 to 12 carbon atoms, which has an alkyl group having 1 to 4 carbon atoms as a branched chain. A polyamide-based polymer, characterized in that a diamine represented by the following formula (1) is used in combination with the polyamide-based polymer: (2) The polyamide-based polymer according to (1) above, wherein terephthalic acid or a salt thereof is further used as the dicarboxylic acid, and the terephthalic acid or a salt thereof is used in combination with itaconic acid. (3) The polyamide-based polymer according to (1) or (2), wherein the molar ratio of the diamine represented by formula (I) to the diamine represented by formula (II) [diamine represented by formula (I) / diamine represented by formula (II)] is 5 / 95 to 95 / 5. (4) The method for producing a polyamide-based polymer according to (1) above, wherein the dicarboxylic acid is itaconic acid, and the diamine is a compound represented by the formula (I): H2N-R 1 -NH2(I) (In the formula, R 1 represents a straight-chain alkylene group having 6 to 12 carbon atoms. and a diamine represented by formula (II): H2N-R 2 -NH2(II) (In the formula, R 2 represents an alkylene group having 6 to 12 carbon atoms, which has an alkyl group having 1 to 4 carbon atoms as a branched chain. a diamine represented by formula (I) and a diamine represented by formula (II) are reacted with itaconic acid, and the diamine represented by formula (II) is polymerized to obtain a reaction product. (5) A method for producing a polyamide-based polymer according to (2) above, wherein the dicarboxylic acid is itaconic acid and terephthalic acid or a salt thereof, and the diamine is a compound represented by the formula (I): H2N-R 1 -NH2(I) (In the formula, R 1 represents a straight-chain alkylene group having 6 to 12 carbon atoms. and a diamine represented by formula (II): H2N-R 2 -NH2(II) (In the formula, R 2 represents an alkylene group having 6 to 12 carbon atoms, which has an alkyl group having 1 to 4 carbon atoms as a branched chain. a diamine represented by the formula (I) and a diamine represented by the formula (II), reacting itaconic acid and terephthalic acid or a salt thereof with the diamine represented by the formula (I) and the diamine represented by the formula (II), and polymerizing the obtained reaction product; (6) The method for producing a polyamide-based polymer according to (4) or (5) above, wherein the molar ratio of the diamine represented by formula (I) to the diamine represented by formula (II) [diamine represented by formula (I) / diamine represented by formula (II)] is 5 / 95 to 95 / 5. (7) A polyamide fiber containing the polyamide polymer according to any one of (1) to (3) above, and (8) A molding material containing the polyamide polymer according to any one of (1) to (3) above. Regarding. Effect of the Invention

[0009] According to the present invention, itaconic acid, which is available as a bio-based monomer, is used as a raw material to provide a polyamide-based polymer which has appropriate water resistance, as well as degradability in water and durability, and mechanical strength comparable to that of nylon, and which can serve as a substitute for nylon. [Brief description of the drawings]

[0010] [Figure 1] 1 is a graph showing the nuclear magnetic resonance (1H-NMR) spectrum of the polyamide-based polymer obtained in Example 1. [Diagram 2] 1 is a graph showing the nuclear magnetic resonance (1H-NMR) spectrum of the polyamide-based polymer obtained in Example 1. [Diagram 3] 1 is a graph showing an infrared absorption spectrum of the polyamide-based polymer obtained in Example 1. [Figure 4] 1 is a graph showing the nuclear magnetic resonance (1H-NMR) spectrum of the polyamide-based polymer obtained in Example 4. [Diagram 5] 1 is a graph showing the nuclear magnetic resonance (1H-NMR) spectrum of the polyamide-based polymer obtained in Example 7. [Figure 6] 1 is a graph showing the nuclear magnetic resonance (1H-NMR) spectrum of the polyamide-based polymer obtained in Example 8. [Figure 7]1 is a graph showing the nuclear magnetic resonance (1H-NMR) spectrum of the polyamide-based polymer obtained in Example 12. [Figure 8] 1 is a graph showing an infrared absorption spectrum of the polyamide-based polymer obtained in Example 14. [Figure 9] 1 is a graph showing the results of accelerated light fastness testing of Polymer D, Polymer S, Polymer X and Polymer Y. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] (1) Polyamide polymer A As described above, the polyamide-based polymer of the present invention is a polyamide-based polymer obtained by polymerizing a dicarboxylic acid and a diamine, in which itaconic acid is used as the dicarboxylic acid and a diamine is used as the diamine represented by the formula (I): H2N-R 1 -NH2(I) (In the formula, R 1 represents a straight-chain alkylene group having 6 to 12 carbon atoms. and a diamine represented by formula (II): H2N-R 2 -NH2(II) (In the formula, R 2 represents an alkylene group having 6 to 12 carbon atoms, which has an alkyl group having 1 to 4 carbon atoms as a branched chain. The compound is characterized in that it is used in combination with a diamine represented by the following formula:

[0012] The polyamide-based polymer of the present invention uses itaconic acid, a diamine represented by formula (I), and a diamine represented by formula (II), and therefore has appropriate water resistance, as well as degradability and durability in water, and mechanical strength comparable to that of nylon.

[0013] The polyamide polymer of the present invention can be prepared by using itaconic acid as a dicarboxylic acid, and using a diamine represented by formula (I) and a diamine represented by formula (II) as diamines, reacting itaconic acid with the diamine represented by formula (I) and the diamine represented by formula (II), and polymerizing the resulting reaction product. Note that since the polymerization reaction between a dicarboxylic acid and a diamine is a dehydration polycondensation reaction, stoichiometrically, 1 mole of itaconic acid reacts with 1 mole of dicarboxylic acid.

[0014] Itaconic acid can be readily obtained commercially from, for example, Fuso Chemical Industry Co., Ltd., Iwata Chemical Industry Co., Ltd., Cargill, etc. Itaconic acid may be produced using fungi such as Aspergillus terreus, or may be synthesized using petroleum as a raw material. Among these, itaconic acid produced using fungi such as Aspergillus terreus has the advantage of being more environmentally friendly than itaconic acid synthesized using petroleum as a raw material.

[0015] In the diamine represented by formula (I), R 1 R is a linear alkylene group having 6 to 12 carbon atoms. 1 The carbon number of the alkyl group is 6 to 12, preferably an integer of 8 to 10, and more preferably 9, from the viewpoint of obtaining a polyamide-based polymer having appropriate water resistance, as well as degradability and durability in water and mechanical strength comparable to that of nylon.

[0016] Diamines represented by formula (I) include hexanediamine, heptanediamine, octanediamine, nonanediamine, decanediamine and dodecanediamine. These diamines may be used alone or in combination of two or more. Among these diamines, octanediamine, nonanediamine and decanediamine are preferred, and nonanediamine is more preferred, from the viewpoint of obtaining a polyamide-based polymer having appropriate water resistance, decomposability in water, and durability, and mechanical strength comparable to that of nylon.

[0017] In the diamine represented by formula (II), R 2 R is an alkylene group having 6 to 12 carbon atoms and an alkyl group having 1 to 4 carbon atoms as a branched chain. 2 From the viewpoint of obtaining a polyamide-based polymer having appropriate water resistance, biodegradability, and excellent mechanical strength, the carbon number is 6 to 12, preferably an integer of 8 to 10, and more preferably 9.

[0018] R 2 has an alkyl group having 1 to 4 carbon atoms as a branched chain. Examples of the alkyl group having 1 to 4 carbon atoms include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, and a tert-butyl group. Among these alkyl groups, from the viewpoint of obtaining a polyamide-based polymer having appropriate water resistance, biodegradability, and excellent mechanical strength, a methyl group and an ethyl group are preferred, and a methyl group is more preferred.

[0019] Examples of the diamine represented by formula (II) include 2-methyl-1,5-pentanediamine, 3-methyl-1,5-pentanediamine, 3-ethyl-1,5-pentanediamine, 2-methyl-1,6-hexanediamine, 2-ethyl-1,6-hexanediamine, 3-methyl-1,6-hexanediamine, 3-ethyl-1,6-hexanediamine, 2-methyl-1,8-octanediamine, 3-methyl-1,8-octanediamine, 4-methyl-1,8-octanediamine, 2-ethyl-1,8-octanediamine, 3-ethyl-1,8-octanediamine, 4-ethyl-1,8-octanediamine, 3-propyl-1,8-octanediamine, 2-butyl-1,8-octanediamine, 3-butyl-1,8-octanediamine, 4 -butyl-1,8-octanediamine, 2-methyl-1,9-nonanediamine, 3-methyl-1,9-nonanediamine, 4-methyl-1,9-nonanediamine, 2-ethyl-1,9-nonanediamine, 3-ethyl-1,9-nonanediamine, 4-ethyl-1,9-nonanediamine, 2-propyl-1,9-nonanediamine, 3-propyl-1,9-nonanediamine, 4-propyl-1,9-nonanediamine, 2-methyl-1,10-decanediamine, 3-methyl-1,10-decanediamine, 4-methyl-1,10-decanediamine, 2-ethyl-1,10-decanediamine, 3-ethyl-1,10-decanediamine, 4-ethyl-1,10-decanediamine, etc., but the present invention is not limited to only these examples. These diamines may be used alone or in combination of two or more kinds.

[0020] Among the diamines represented by formula (II), from the viewpoint of obtaining a polyamide-based polymer having appropriate water resistance, biodegradability, and excellent mechanical strength, R 2 R is a diamine having an alkyl group having 1 or 2 carbon atoms as a branched chain, and the total carbon number of the molecule is preferably 7 to 11. 2 More preferably, R is a diamine having an alkyl group having 1 or 2 carbon atoms as a branched chain and the total carbon number of the molecule is 7 to 10. 2More preferably, R has an alkyl group having 1 or 2 carbon atoms as a branched chain, and the total carbon number of the molecule is 7 to 11. 2 More preferred is a diamine having methyl groups as branched chains and a total carbon number of 9 in the molecule. More specifically, suitable diamines include 2-methyl-1,6-hexanediamine and 2-methyl-1,8-octanediamine. Among these, 2-methyl-1,8-octanediamine is preferred from the viewpoint of obtaining a polyamide-based polymer having appropriate water resistance, biodegradability, and excellent mechanical strength.

[0021] One of the features of the present invention is that the diamine represented by formula (I) and the diamine represented by formula (II) are used in combination in the present invention. Since the diamine represented by formula (I) and the diamine represented by formula (II) are used in combination in the present invention, a polyamide-based polymer having appropriate water resistance, biodegradability, and excellent mechanical strength can be obtained.

[0022] The molar ratio of the diamine represented by formula (I) to the diamine represented by formula (II) [diamine represented by formula (I) / diamine represented by formula (II)] is preferably 5 / 95 to 95 / 5, more preferably 10 / 90 to 90 / 10, even more preferably 15 / 85 to 85 / 15, still more preferably 20 / 80 to 80 / 20, even more preferably 25 / 75 to 75 / 25, and particularly preferably 30 / 70 to 75 / 25, from the viewpoint of obtaining a polyamide-based polymer having appropriate water resistance, biodegradability, and excellent mechanical strength.

[0023] In addition, diamines other than the diamines represented by formula (I) and formula (II) (hereinafter referred to as other diamines) may be used within the scope that does not impair the object of the present invention. Examples of other diamines include trimethylenediamine, tetramethylenediamine, pentamethylenediamine, phenylenediamine, xylylenediamine, etc., but the present invention is not limited to only these examples.

[0024] Since itaconic acid reacts with the diamine represented by formula (I) and the diamine represented by formula (II) in stoichiometric amounts, the total amount of the diamine represented by formula (I) and the diamine represented by formula (II) is theoretically 1 mole per mole of itaconic acid. Therefore, the total amount of the diamine represented by formula (I) and the diamine represented by formula (II) per mole of itaconic acid is 1 mole. However, when preparing the polyamide-based polymer of the present invention, the amount of itaconic acid may be in excess of the total amount of the diamine represented by formula (I) and the diamine represented by formula (II), and the total amount of the diamine represented by formula (I) and the diamine represented by formula (II) may be in excess of the amount of itaconic acid.

[0025] As described above, the polyamide-based polymer of the present invention can be prepared, for example, by reacting itaconic acid with a diamine represented by formula (I) and a diamine represented by formula (II), and polymerizing the resulting reaction product.

[0026] The reaction of itaconic acid with the diamine represented by formula (I) and the diamine represented by formula (II) can be carried out in an organic solvent, which is preferably a good solvent for itaconic acid and the diamine represented by formula (I) and the diamine represented by formula (II), but a poor solvent for the reaction product.

[0027] Examples of the organic solvent include aliphatic alcohols having 1 to 3 carbon atoms, such as methanol, ethanol, and propanol, ketone compounds, such as acetone and methyl ethyl ketone, ethyl acetate, tetrahydrofuran, dioxane, chloroform, dichloromethane, chlorobenzene, phenol, and cresol, but the present invention is not limited to these examples. These organic solvents may be used alone or in combination of two or more kinds.

[0028] The amount of the organic solvent is not particularly limited as long as it is an amount that allows efficient reaction between itaconic acid and the diamine represented by formula (I) and the diamine represented by formula (II). Generally, however, the amount is preferably about 3 to 20 times, and more preferably about 5 to 15 times, the total amount (mass) of itaconic acid and the diamine represented by formula (I) and the diamine represented by formula (II).

[0029] The reaction temperature when itaconic acid is reacted with the diamine represented by formula (I) and the diamine represented by formula (II) is not particularly limited, but is preferably about 40 to 60°C from the viewpoint of increasing the reaction efficiency. The reaction time when itaconic acid is reacted with the diamine represented by formula (I) and the diamine represented by formula (II) varies depending on the amount of the organic solvent used, the reaction temperature, etc., so it cannot be determined in general, but is usually about 1.5 to 3 hours. The atmosphere when itaconic acid is reacted with the diamine represented by formula (I) and the diamine represented by formula (II) is not particularly limited, and may be air or an inert gas such as nitrogen gas or argon gas.

[0030] After the reaction is completed, the reaction product is crystallized from the obtained reaction mixture. Examples of methods for crystallizing the reaction product from the reaction mixture include a method of cooling the reaction mixture to a temperature of about 0 to 25° C., a method of gradually dropping a poor solvent such as hexane, toluene, or xylene into the reaction mixture, and a method of gradually evaporating the solvent contained in the reaction mixture, but the present invention is not limited to only these methods.

[0031] The crystallized reaction product can be collected by a method such as filtration, etc. The collected reaction product may be washed with a non-organic solvent having a temperature of about 0 to 25° C., if necessary.

[0032] Next, the reaction product obtained above is polymerized to obtain the polyamide polymer of the present invention.

[0033] Examples of the method for polymerizing the reaction product include bulk polymerization, suspension polymerization, and emulsion polymerization, but the present invention is not limited to these examples. Among these polymerization methods, bulk polymerization is preferred from the viewpoint of efficiently preparing a polyamide-based polymer with a small amount of impurities. When preparing a polyamide-based polymer by bulk polymerization, the reaction product obtained above is heated to a polymerization temperature of about 150 to 250°C and polymerized to obtain a polyamide-based polymer. The atmosphere in which the reaction product obtained above is polymerized is not particularly limited, and may be air or an inert gas such as nitrogen gas or argon gas.

[0034] In addition, when polymerizing the reaction product, it is preferable to use an appropriate amount of catalyst from the viewpoint of efficiently preparing a polyamide-based polymer. Examples of the catalyst include sodium dihydrogen phosphate, disodium hydrogen phosphate, trisodium phosphate, potassium dihydrogen phosphate, dipotassium hydrogen phosphate, tripotassium phosphate, lithium dihydrogen phosphate, dilithium hydrogen phosphate, and trilithium phosphate, but the present invention is not limited to these examples. Among the catalysts, sodium dihydrogen phosphate is preferable.

[0035] The reaction product is polymerized as described above to obtain a polyamide-based polymer. The polyamide-based polymer obtained above may be purified, if necessary, by dissolving it in a solvent such as N,N-dimethylformamide, and then precipitating it with a ketone compound such as acetone. The polyamide-based polymer obtained above may be dried, for example, by drying under reduced pressure.

[0036] The polyamide-based polymer obtained as described above has the formula (IIIa):

[0037] [ka]

[0038] (In the formula, p represents an integer of 6 to 12.) and a repeating unit represented by formula (IIIb):

[0039] [ka]

[0040] (In the formula, R 2 is the same as above) The polyamide polymer of the present invention may contain repeating units other than the repeating units represented by formula (IIIa) and the repeating units represented by formula (IIIb) within the scope of the present invention.

[0041] In the present invention, since the polymer has a repeating unit represented by formula (IIIa) and a repeating unit represented by formula (IIIb), the polymer has appropriate water resistance, as well as degradability and durability in water, and mechanical strength comparable to that of nylon.

[0042] The molar ratio of the repeating unit represented by formula (IIIa) to the repeating unit represented by formula (IIIb) [repeating unit represented by formula (IIIa) / repeating unit represented by formula (IIIb)] is substantially the same as the molar ratio of the diamine represented by formula (I) to the diamine represented by formula (II) [diamine represented by formula (I) / diamine represented by formula (II)].

[0043] Therefore, the molar ratio of the repeating unit represented by formula (IIIa) to the repeating unit represented by formula (IIIb) [repeating unit represented by formula (IIIa) / repeating unit represented by formula (IIIb)] is preferably 5 / 95 to 95 / 5, more preferably 10 / 90 to 90 / 10, even more preferably 15 / 85 to 85 / 15, still more preferably 20 / 80 to 80 / 20, even more preferably 25 / 75 to 75 / 25, and particularly preferably 30 / 70 to 75 / 25, from the viewpoints of imparting appropriate water resistance and biodegradability to the polyamide-based polymer and enhancing the mechanical strength of the polyamide-based polymer.

[0044] The content of the repeating unit represented by formula (IIIa) in the polyamide-based polymer of the present invention is preferably 5 to 95 mol%, more preferably 10 to 90 mol%, even more preferably 15 to 85 mol%, still more preferably 20 to 80 mol%, even more preferably 25 to 75 mol%, and particularly preferably 30 to 75 mol%, from the viewpoint of imparting suitable water resistance and biodegradability to the polyamide-based polymer and increasing the mechanical strength of the polyamide-based polymer. The content of the repeating unit represented by formula (IIIb) in the polyamide-based polymer of the present invention is preferably 5 to 95 mol%, more preferably 10 to 90 mol%, even more preferably 15 to 85 mol%, even more preferably 20 to 80 mol%, even more preferably 25 to 75 mol%, and particularly preferably 25 to 70 mol%, from the viewpoint of imparting suitable water resistance and biodegradability to the polyamide-based polymer and increasing the mechanical strength of the polyamide-based polymer.

[0045] In the polyamide-based polymer of the present invention, the repeating unit represented by formula (IIIa) and the repeating unit represented by formula (IIIb) are usually present randomly, but may be present alternately or in a block form.

[0046] The number average molecular weight of the polyamide-based polymer of the present invention is not particularly limited, but from the viewpoint of imparting appropriate water resistance and biodegradability to the polyamide-based polymer and increasing the mechanical strength of the polyamide-based polymer, it is preferably 15,000 to 800,000, and more preferably 20,000 to 100,000. The number average molecular weight of the polyamide-based polymer is a value measured based on the method described in the following examples.

[0047] (2) Polyamide polymer B In the present invention, even when terephthalic acid (salt) is not used, a polyamide-based polymer having appropriate water resistance, as well as degradability and durability in water, and mechanical strength comparable to that of nylon can be obtained. However, from the viewpoint of imparting appropriate water resistance and biodegradability to the polyamide-based polymer and improving the decomposition in water, mechanical strength, and heat resistance of the polyamide-based polymer, it is preferable to use terephthalic acid or a salt thereof (hereinafter referred to as terephthalic acid (salt)) in addition to itaconic acid as the dicarboxylic acid.

[0048] The polyamide-based polymer of the present invention uses itaconic acid and terephthalic acid (salt) as the dicarboxylic acid, and the diamine represented by formula (I) and the diamine represented by formula (II) as the diamine, and therefore has appropriate water resistance, is biodegradable, has good decomposition ability in water, and is excellent in mechanical strength and heat resistance.

[0049] The polyamide-based polymer can be obtained, for example, by using itaconic acid and terephthalic acid (salt) as dicarboxylic acids and using a diamine represented by formula (I) and a diamine represented by formula (II) as diamines, reacting the itaconic acid and terephthalic acid (salt) with the diamine represented by formula (I) and the diamine represented by formula (II), and polymerizing the obtained reaction product.

[0050] Examples of terephthalic acid (salts) include terephthalic acid, terephthalic acid di-alkali metal salts such as disodium terephthalate and dipotassium terephthalate, but the present invention is not limited to these examples. These terephthalic acids (salts) may be used alone or in combination of two or more. Among terephthalic acids (salts), terephthalic acid is preferred from the viewpoint of increasing the purity of the polyamide polymer.

[0051] Itaconic acid and terephthalic acid (salt) react with the diamine represented by formula (I) and the diamine represented by formula (II) in stoichiometric amounts. Therefore, theoretically, 1 mole of the diamine represented by formula (I) and the diamine represented by formula (II) reacts with 1 mole of the itaconic acid and terephthalic acid (salt) in total. For this reason, in the present invention, when terephthalic acid (salt) is used as a dicarboxylic acid in addition to itaconic acid, a part of the itaconic acid in the polyamide polymer A is replaced with terephthalic acid (salt).

[0052] The molar ratio of itaconic acid to terephthalic acid (salt) [itaconic acid / terephthalic acid (salt)] is preferably 0 / 100 to 95 / 5, more preferably 5 / 95 to 95 / 5, even more preferably 5 / 95 to 85 / 15, still more preferably 10 / 90 to 80 / 20, even more preferably 15 / 85 to 70 / 30, and particularly preferably 20 / 80 to 60 / 40, from the viewpoints of imparting appropriate water resistance and biodegradability to the polyamide-based polymer and further improving the decomposition property and heat resistance of the polyamide-based polymer in water.

[0053] As described above, from the viewpoints of imparting suitable water resistance and biodegradability to the polyamide-based polymer and enhancing the mechanical strength of the polyamide-based polymer, the molar ratio of the diamine represented by formula (I) to the diamine represented by formula (II) [diamine represented by formula (I) / diamine represented by formula (II)] is preferably 5 / 95 to 95 / 5, more preferably 10 / 90 to 90 / 10, even more preferably 15 / 85 to 85 / 15, still more preferably 20 / 80 to 80 / 20, even more preferably 25 / 75 to 75 / 25, and particularly preferably 30 / 70 to 75 / 25.

[0054] Since itaconic acid and terephthalic acid (salt) react with the diamine represented by formula (I) and the diamine represented by formula (II) in stoichiometric amounts, the total amount of the diamine represented by formula (I) and the diamine represented by formula (II) is theoretically 1 mole per mole of the total amount of itaconic acid and terephthalic acid (salt). Therefore, the total amount of the diamine represented by formula (I) and the diamine represented by formula (II) per mole of the total amount of itaconic acid and terephthalic acid (salt) is 1 mole. However, when preparing the polyamide-based polymer of the present invention, the total amount of itaconic acid and terephthalic acid (salt) may be in excess of the total amount of the diamine represented by formula (I) and the diamine represented by formula (II), and the total amount of the diamine represented by formula (I) and the diamine represented by formula (II) may be in excess of the total amount of itaconic acid and terephthalic acid (salt).

[0055] The reaction of itaconic acid and terephthalic acid (salt) with the diamine represented by formula (I) and the diamine represented by formula (II) can be carried out in an organic solvent. The organic solvent is preferably a good solvent for itaconic acid, terephthalic acid (salt), the diamine represented by formula (I) and the diamine represented by formula (II), and a poor solvent for the resulting reaction product. Examples of the organic solvent include the same ones as those used when preparing the polyamide polymer A.

[0056] The amount of the organic solvent is not particularly limited as long as it is an amount that allows efficient reaction between the itaconic acid and terephthalic acid (salt), the diamine represented by formula (I), and the diamine represented by formula (II), but it is usually preferably about 3 to 20 times, and more preferably about 5 to 15 times, the total amount (mass) of the itaconic acid, terephthalic acid (salt), the diamine represented by formula (I), and the diamine represented by formula (II).

[0057] The reaction temperature when reacting itaconic acid and terephthalic acid (salt) with the diamine represented by formula (I) and the diamine represented by formula (II) is not particularly limited, but is preferably about 60 to 90°C from the viewpoint of increasing the reaction efficiency. The reaction time when reacting itaconic acid and terephthalic acid (salt) with the diamine represented by formula (I) and the diamine represented by formula (II) varies depending on the amount of the organic solvent used, the reaction temperature, etc., so it cannot be determined in general, but is usually about 1.5 to 3 hours. The atmosphere when reacting itaconic acid and terephthalic acid (salt) with the diamine represented by formula (I) and the diamine represented by formula (II) is not particularly limited, and may be air, or may be an inert gas such as nitrogen gas or argon gas.

[0058] After the reaction is completed, the reaction product is crystallized from the obtained reaction mixture. Examples of methods for crystallizing the reaction product from the reaction mixture include a method of cooling the reaction mixture to a temperature of about 0 to 25°C, a method of gradually dropping a poor solvent such as hexane, toluene, or xylene into the reaction mixture, and a method of gradually evaporating the solvent contained in the reaction mixture, but the present invention is not limited to only such methods. The generated reaction product can be recovered, for example, by filtration. The recovered reaction product may be washed with a non-polar organic solvent having a temperature of about 0 to 25°C, if necessary.

[0059] Next, the reaction product obtained above is polymerized to obtain the polyamide polymer of the present invention.

[0060] Examples of the method for polymerizing the reaction product include bulk polymerization, suspension polymerization, and emulsion polymerization, but the present invention is not limited to these examples. Among these polymerization methods, bulk polymerization is preferred from the viewpoint of efficiently preparing a polyamide-based polymer with a small amount of impurities. When preparing a polyamide-based polymer by bulk polymerization, the reaction product obtained above is heated to a polymerization temperature of about 150 to 250°C and polymerized to obtain a polyamide-based polymer. The atmosphere in which the reaction product obtained above is polymerized is not particularly limited, and may be air or an inert gas such as nitrogen gas or argon gas.

[0061] In addition, when polymerizing the reaction product, it is preferable to use a suitable amount of a catalyst from the viewpoint of efficiently preparing a polyamide-based polymer. Examples of the catalyst include those mentioned above.

[0062] The reaction product is polymerized as described above to obtain a polyamide-based polymer. The polyamide-based polymer obtained above may be purified, if necessary, by dissolving it in a solvent such as N,N-dimethylformamide, and then precipitating it with a ketone compound such as acetone. The polyamide-based polymer obtained above may be dried, for example, by drying under reduced pressure.

[0063] The polyamide-based polymer obtained as described above further contains a repeating unit represented by the formula (IIIc) in addition to the repeating unit represented by the formula (IIIa) and the repeating unit represented by the formula (IIIb): Formula (Ic):

[0064] [ka]

[0065] (wherein p is the same as above) and a repeating unit represented by formula (IIId):

[0066] [ka]

[0067] (In the formula, R 2 is the same as above) The polyamide polymer of the present invention may contain repeating units other than the repeating units represented by formula (IIIa), (IIIb), (IIIc) and (IIId) within the scope of the object of the present invention.

[0068] The polyamide-based polymer of the present invention has a repeating unit represented by formula (IIIc) and a repeating unit represented by formula (IIId) in addition to the repeating unit represented by formula (IIIa) and the repeating unit represented by formula (IIIb), and therefore has appropriate water resistance and biodegradability, good decomposition in water, and excellent heat resistance.

[0069] Since itaconic acid and terephthalic acid (salts) react with the diamine represented by formula (I) and the diamine represented by formula (II) in stoichiometric amounts, the total content of units derived from itaconic acid and units derived from terephthalic acid (salts) in the polyamide-based polymer of the present invention is 50 mol%, and the total content of units derived from the diamine represented by formula (I) and units derived from the diamine represented by formula (II) in the polyamide-based polymer of the present invention is 50 mol%.

[0070] Therefore, in the polyamide-based polymer of the present invention, the formula (IV):

[0071] [ka]

[0072] Units and formula (V):

[0073] [ka] The total content of the unit represented by formula (IV) and the unit represented by formula (V) is 50 mol %. The unit represented by formula (IV) is a unit derived from itaconic acid, and the unit represented by formula (V) is a unit derived from terephthalic acid (salt).

[0074] The molar ratio of the repeating units represented by formula (IIIa) and (IIIb) to the repeating units represented by formula (IIIc) and (IIId) [repeating units represented by formula (IIIa) and (IIIb) / repeating units represented by formula (IIIc) and (IIId)] is substantially the same as the molar ratio of itaconic acid to terephthalic acid (salt) described above [itaconic acid / terephthalic acid (salt)].

[0075] Therefore, the molar ratio of the repeating units represented by formula (IIIa) and (IIIb) to the repeating units represented by formula (IIIc) and (IIId) [repeating units represented by formula (IIIa) and (IIIb) / repeating units represented by formula (IIIc) and (IIId)] is preferably 0 / 100 to 95 / 5, more preferably 5 / 95 to 95 / 5, even more preferably 5 / 95 to 85 / 15, even more preferably 10 / 90 to 80 / 20, even more preferably 15 / 85 to 70 / 30, and even more preferably 20 / 80 to 60 / 40, from the viewpoints of imparting appropriate water resistance and biodegradability to the polyamide-based polymer and further improving the decomposition property in water and heat resistance of the polyamide-based polymer.

[0076] The ratio of the total moles of the repeating units represented by formula (IIIa) and the repeating units represented by formula (IIIc) to the total moles of the repeating units represented by formula (IIIb) and the repeating units represented by formula (IIId) is substantially the same as the molar ratio of the diamine represented by formula (I) to the diamine represented by formula (II). The repeating units represented by formula (IIIa) and the repeating units represented by formula (IIIc) are units derived from the diamine represented by formula (I). The repeating units represented by formula (IIIb) and the repeating units represented by formula (IIId) are units derived from the diamine represented by formula (II).

[0077] Therefore, the ratio of the total moles of the repeating units represented by formula (IIIa) and the repeating units represented by formula (IIIc) to the total moles of the repeating units represented by formula (IIIb) and the repeating units represented by formula (IIId) [total moles of the repeating units represented by formula (IIIa) and the repeating units represented by formula (IIIc) / total moles of the repeating units represented by formula (IIIb) and the repeating units represented by formula (IIId)] is preferably 5 / 95 to 95 / 5, more preferably 10 / 90 to 90 / 10, even more preferably 15 / 85 to 85 / 15, still more preferably 20 / 80 to 80 / 20, even more preferably 25 / 75 to 75 / 25, and particularly preferably 30 / 70 to 75 / 25, from the viewpoints of imparting appropriate water resistance and biodegradability to the polyamide-based polymer and enhancing the mechanical strength of the polyamide-based polymer.

[0078] The total content of the repeating unit represented by formula (IIIa) and the repeating unit represented by formula (IIIc) in the polyamide-based polymer of the present invention is, from the viewpoints of imparting appropriate water resistance and biodegradability to the polyamide-based polymer and increasing the mechanical strength of the polyamide-based polymer, preferably 5 to 95 mol %, more preferably 10 to 90 mol %, even more preferably 15 to 85 mol %, still more preferably 20 to 80 mol %, even more preferably 25 to 75 mol %, and particularly preferably 30 to 75 mol %. The total content of the repeating unit represented by formula (IIIb) and the repeating unit represented by formula (IIId) in the polyamide-based polymer of the present invention is, from the viewpoints of imparting appropriate water resistance and biodegradability to the polyamide-based polymer and increasing the mechanical strength of the polyamide-based polymer, preferably 5 to 95 mol %, more preferably 10 to 90 mol %, even more preferably 15 to 85 mol %, still more preferably 20 to 80 mol %, even more preferably 25 to 75 mol %, and particularly preferably 25 to 70 mol %.

[0079] In the polyamide polymer of the present invention, the repeating unit represented by formula (IIIa), the repeating unit represented by formula (IIIb), the repeating unit represented by formula (IIIc) and the repeating unit represented by formula (IIId) are usually present randomly, but may be present alternately or in a block form.

[0080] The number average molecular weight of the polyamide-based polymer obtained above is not particularly limited, but from the viewpoint of imparting appropriate water resistance and biodegradability to the polyamide-based polymer and enhancing the decomposition property of the polyamide-based polymer in water and improving the heat resistance, it is preferably 15,000 to 800,000, and more preferably 20,000 to 650,000. The number average molecular weight of the polyamide-based polymer is a value measured based on the method described in the following examples.

[0081] (3) Applications of polyamide polymers Since the polyamide-based polymer of the present invention is soluble in an organic solvent, a spinning dope can be prepared by dissolving the polyamide-based polymer in an organic solvent. Examples of the organic solvent include those mentioned above.

[0082] The amount of the organic solvent relative to the polyamide-based polymer of the present invention cannot be determined in general because it varies depending on the type of the organic solvent, etc. Usually, it is preferable to add the organic solvent to the polyamide-based polymer so that the spinning dope has a desired viscosity.

[0083] The thus obtained spinning dope is extruded through the holes of the spinneret, and the organic solvent is removed by volatilization, whereby polyamide fibers can be produced.

[0084] In addition, since the polyamide-based polymer of the present invention has thermoplastic properties, the polyamide-based polymer can be melt-spun by heating and melting the polyamide-based polymer and injecting it from a fine hole in a spinneret using a melt spinning device.

[0085] The spinneret is generally made of an alloy such as an alloy of gold and platinum, an alloy of platinum and iridium, or an alloy of platinum and palladium. The hole diameter of the spinneret is appropriately determined according to the fineness of the target polyamide fiber, but is usually about 0.05 to 0.1 mm. The number of holes provided in the spinneret is not particularly limited, but is usually about 1 to 20,000.

[0086] The polyamide fiber may be a single fiber (filament), or may be a fiber formed by bundling a plurality of single fibers extruded from a plurality of holes.

[0087] The polyamide fibers obtained as described above may be subjected to treatments such as washing, drying and crimping, if necessary.

[0088] The fineness of the polyamide fiber obtained above varies depending on the application of the polyamide fiber and cannot be generally determined, so it is preferable to appropriately determine it depending on the application of the polyamide fiber. An example of the fineness of the polyamide fiber is 1 to 30 decitex, but the present invention is not limited by the fineness. The fineness of the polyamide fiber can be easily adjusted by adjusting the hole diameter of the spinneret or adjusting the draw ratio when drawing the polyamide fiber.

[0089] The polyamide fiber obtained above may be stretched as necessary to increase the mechanical strength. The stretching of the polyamide fiber is usually uniaxial stretching, but may be biaxial stretching.

[0090] The polyamide-based fibers may be used in the form of long fibers, or may be cut to a desired fiber length and used as short fibers. The fiber length of the polyamide-based fibers varies depending on the application of the polyamide-based fibers, and is therefore preferably determined appropriately depending on the application of the polyamide-based fibers.

[0091] The polyamide fibers may be used for fishing lines and the like, and may also be used for knitted fabrics such as woven fabrics, nonwoven fabrics, and fishing nets.

[0092] The knitted fabric can be manufactured using the polyamide-based fibers and a knitting machine or the like. When manufacturing the knitted fabric, the polyamide-based fibers may be used as they are, or, for example, a blend of the polyamide-based fibers with synthetic fibers such as polyester fibers and acrylic fibers, or fibers such as cotton yarn, wool yarn, and raw silk may be used. Examples of knitted fabrics include flat knitting, rib knitting, and purl knitting, but the present invention is not limited to these examples.

[0093] The woven fabric can be manufactured by using the polyamide fibers as the warp, weft, or both the warp and weft, using a loom or the like. The woven fabric may be a blended fabric in which blended yarns containing polyamide fibers are used in some or all of the warp and weft, a union fabric in which the warp and weft have different compositions and polyamide fibers are used in the warp and / or weft, or a highly woven fabric in which warp and weft containing the polyamide fibers of the present invention and having different fiber diameters are used. Examples of the weave of the woven fabric include a plain weave, a twill weave, a twill weave, a satin weave, and a variation weave, but the present invention is not limited to these examples.

[0094] The nonwoven fabric can be manufactured by a dry method or a wet method using fibers containing the polyamide fibers. The fibers used in the nonwoven fabric may be only the polyamide fibers, or may be a blend of the polyamide fibers with synthetic fibers such as polyester fibers and acrylic fibers, cotton yarns, wool yarns, raw silk, and other fibers. Examples of the dry method include mechanical bonding methods such as the chemical pond method, the thermal pond method, the needle punch method, and the airlaid method, but the present invention is not limited to these examples. Examples of the wet method include the hydroentanglement method, but the present invention is not limited to these examples.

[0095] Since the polyamide-based fiber uses the polyamide-based polymer of the present invention, it has appropriate water resistance, biodegradability, and excellent mechanical strength. Therefore, it can be used not only for fishing equipment such as fishing nets and fishing lines in the fishing industry, agricultural equipment, and the like, but also for various other applications such as clothing such as gloves, underwear, socks, shirts, and Western clothing, as well as face masks, materials for disposable diapers, and cosmetic sheets such as lotion wipes.

[0096] In addition, since the polyamide-based polymer of the present invention is soluble in an organic solvent, it can be used as an organic solvent solution, and since it has thermoplasticity, it can be used as a molten material melted by heating. Therefore, the polyamide-based polymer of the present invention can be suitably used as a molding material such as an injection molding material.

[0097] The polyamide polymer of the present invention may contain an appropriate amount of additives depending on the application, if necessary. Examples of additives include colorants such as pigments and dyes, ultraviolet absorbers, ultraviolet stabilizers, antioxidants, rust inhibitors, antibacterial agents, plasticizers, algae inhibitors, fungicides, flame retardants, and foaming agents, but the present invention is not limited to these examples. These additives may be used alone or in combination of two or more types. The amount of additives varies depending on the type of additive, so it cannot be determined in general, and it is preferable to determine the amount appropriately depending on the type of additive. EXAMPLES

[0098] Next, the present invention will be described in more detail based on examples, but the present invention is not limited to these examples.

[0099] The physical properties of the polymers obtained in the following Examples and Comparative Examples were examined according to the following methods.

[0100] [Polymer structure] The structure of the polymer was determined by nuclear magnetic resonance ( 1 The NMR spectroscopy (H-NMR) was used to determine the 1 H-NMR was performed using a nuclear magnetic resonance spectrometer (Bruker, product name: AVANCE III 400, 400 MHz) by dissolving 5 mg of a sample (polymer) in 0.5 mL of dimethylsulfoxide-d6, transferring the resulting solution to a glass sample tube, and measuring at a temperature of 25°C with an accumulation number of 16.

[0101] [Number average molecular weight of polymer] The number average molecular weight of the polymer was measured by gel permeation chromatography (GPC). More specifically, the measurement was performed using a GPC measuring device equipped with two columns (Shodex KD-803 and Shodex KD-804, manufactured by Showa Denko K.K.) as the equipment. The external standard was pullulan.

[0102] Polymer Properties (1) Differential scanning calorimetry (DSC) The differential scanning calorimetry was performed using a differential scanning calorimeter (manufactured by Seiko Instruments Inc., trade name: EXSTAE6100) in a nitrogen gas atmosphere at temperatures of 25 to 200° C. at a heating rate of 10° C. / min.

[0103] (2) Thermogravimetric analysis (TGA) and 10% weight loss temperature Thermogravimetric analysis was performed using a thermogravimetric analyzer (Seiko Instruments Inc., product name: SSC / 5200SII) in a nitrogen gas atmosphere at a temperature rise rate of 10°C / min at temperatures of 30 to 800°C. Based on the results of the thermogravimetric analysis, the 10% weight loss temperature was determined. The 10% weight loss temperature refers to the temperature at which the mass of the sample (polymer) decreases by 10%.

[0104] (3) Uniaxial tensile strength of polymer The uniaxial tensile strength of a polymer was measured by pulling a 10 mm long fibrous sample (polymer) at room temperature with a tensile tester (Instron, product number: 3365-L5) at a crosshead speed of 1 mm / sec. Young's modulus was determined from the initial slope of the stress-strain curve.

[0105] Example 1 A mixed solution was obtained by slowly adding 1 mol of a diamine consisting of 92 mol % of n-nonanediamine and 8 mol % of 2-methyl-1,8-octanediamine to 200 mL of an ethanol solution containing 1 mol (13 g) of itaconic acid over a period of 2 hours at a liquid temperature of 45° C. while stirring.

[0106] The mixture solution obtained above was cooled to 25° C. to precipitate a white solid reaction product (yield: 96% by mass). The mixture solution was filtered to collect the reaction product, which was washed with ethanol at about 10° C. and then dried in a vacuum dryer at 45° C. for 12 hours.

[0107] Next, 20 g of the reaction product obtained above was mixed with 0.2 g of sodium dihydrogen phosphate as a catalyst, and the resulting mixture was heated to 190°C under reduced pressure to polymerize the reaction product for 6 hours, thereby obtaining a polyamide-based polymer.

[0108] The polyamide-based polymer obtained above was dissolved in N,N-dimethylformamide, and the resulting solution was added to acetone to purify the polyamide-based polymer. The polyamide-based polymer was then washed with acetone and dried in a vacuum dryer at 120°C for approximately 24 hours to obtain a purified polyamide-based polymer (hereinafter referred to as polymer A) (yield: 92% by mass).

[0109] The number average molecular weight of the polymer A obtained above was 24,500. 1 The H-NMR) spectra are shown in Figures 1 and 2. In Figure 1, DMSO was measured by nuclear magnetic resonance ( 1 The H-NMR spectrum was measured using dimethyl sulfoxide, which was the solvent used. The infrared absorption spectrum of polymer A is shown in Figure 3.

[0110] Example 2 A mixed solution was obtained by slowly adding 1 mol of a diamine consisting of 93 mol % of n-nonanediamine and 7 mol % of 2-methyl-1,8-octanediamine to 200 mL of an ethanol solution containing 1 mol (13 g) of itaconic acid over a period of 2 hours at a liquid temperature of 45° C. with stirring.

[0111] The mixture solution obtained above was cooled to 25° C. to precipitate a white solid reaction product (yield: 96% by mass). The mixture solution was filtered to collect the reaction product, which was washed with ethanol at about 10° C. and then dried in a vacuum dryer at 45° C. for 12 hours.

[0112] Next, 20 g of the reaction product obtained above was mixed with 0.2 g of sodium dihydrogen phosphate as a catalyst, and the resulting mixture was heated to 190°C under reduced pressure to polymerize the reaction product for 6 hours, thereby obtaining a polyamide-based polymer.

[0113] The polyamide-based polymer obtained above was dissolved in N,N-dimethylformamide, and the resulting solution was added to acetone to purify the polyamide-based polymer. The polyamide-based polymer was then washed with acetone and dried in a vacuum dryer at 120°C for approximately 24 hours to obtain a purified polyamide-based polymer (hereinafter referred to as polymer B) (yield: 92% by mass).

[0114] The number average molecular weight of the polymer B obtained above was 23,400. 1 The 1 H-NMR spectrum and infrared absorption spectrum were similar to those of polymer A.

[0115] Example 3 To 200 mL of an ethanol solution containing 1 mol (13 g) of itaconic acid, 1 mol of a diamine consisting of 75 mol % of n-nonanediamine and 25 mol % of 2-methyl-1,8-octanediamine was slowly added over a period of 2 hours at a liquid temperature of 45° C. under stirring to obtain a mixed solution.

[0116] The mixture solution obtained above was cooled to 25° C. to precipitate a white solid reaction product (yield: 96% by mass). The mixture solution was filtered to collect the reaction product, which was washed with ethanol at about 10° C. and then dried in a vacuum dryer at 45° C. for 12 hours.

[0117] Next, 20 g of the reaction product obtained above was mixed with 0.2 g of sodium dihydrogen phosphate as a catalyst, and the resulting mixture was heated to 190°C under reduced pressure to polymerize the reaction product for 6 hours, thereby obtaining a polyamide-based polymer.

[0118] The polyamide-based polymer obtained above was dissolved in N,N-dimethylformamide, and the resulting solution was added to acetone to purify the polyamide-based polymer. The polyamide-based polymer was then washed with acetone and dried in a vacuum dryer at 120°C for approximately 24 hours to obtain a purified polyamide-based polymer (hereinafter referred to as polymer C) (yield: 92% by mass).

[0119] The number average molecular weight of the polymer C obtained above was 38,700. 1 The 1 H-NMR spectrum and infrared absorption spectrum were similar to those of polymer A.

[0120] Example 4 A mixed solution was obtained by slowly adding 1 mol of a diamine consisting of 56% n-nonanediamine and 44 mol % 2-methyl-1,8-octanediamine to 200 mL of an ethanol solution containing 1 mol (13 g) of itaconic acid over a period of 2 hours at a liquid temperature of 45° C. with stirring.

[0121] The mixture solution obtained above was cooled to 25° C. to precipitate a white solid reaction product (yield: 96% by mass). The mixture solution was filtered to collect the reaction product, which was washed with ethanol at about 10° C. and then dried in a vacuum dryer at 45° C. for 12 hours.

[0122] Next, 20 g of the reaction product obtained above was mixed with 0.2 g of sodium dihydrogen phosphate as a catalyst, and the resulting mixture was heated to 190°C under reduced pressure to polymerize the reaction product for 6 hours, thereby obtaining a polyamide-based polymer.

[0123] The polyamide-based polymer obtained above was dissolved in N,N-dimethylformamide, and the resulting solution was added to acetone to purify the polyamide-based polymer. The polyamide-based polymer was then washed with acetone and dried in a vacuum dryer at 120°C for approximately 24 hours to obtain a purified polyamide-based polymer (hereinafter referred to as polymer D) (yield: 92% by mass).

[0124] The number average molecular weight of the polymer D obtained above was 23,400. 1 The H-NMR spectrum is shown in Figure 4. The infrared absorption spectrum of polymer D was similar to that of polymer A.

[0125] Example 5 A mixed solution was obtained by slowly adding 1 mol of a diamine consisting of 34 mol % of n-nonanediamine and 66 mol % of 2-methyl-1,8-octanediamine to 200 mL of an ethanol solution containing 1 mol (13 g) of itaconic acid over a period of 2 hours at a liquid temperature of 45° C. with stirring.

[0126] The mixture solution obtained above was cooled to 25° C. to precipitate a white solid reaction product (yield: 96% by mass). The mixture solution was filtered to collect the reaction product, which was washed with ethanol at about 10° C. and then dried in a vacuum dryer at 45° C. for 12 hours.

[0127] Next, 20 g of the reaction product obtained above was mixed with 0.2 g of sodium dihydrogen phosphate as a catalyst, and the resulting mixture was heated to 190°C under reduced pressure to polymerize the reaction product for 6 hours, thereby obtaining a polyamide-based polymer.

[0128] The polyamide-based polymer obtained above was dissolved in N,N-dimethylformamide, and the resulting solution was added to acetone to purify the polyamide-based polymer. The polyamide-based polymer was then washed with acetone and dried in a vacuum dryer at 120°C for approximately 24 hours to obtain a purified polyamide-based polymer (hereinafter referred to as Polymer E) (yield: 92% by mass).

[0129] The number average molecular weight of the polymer E obtained above was 49,600. 1 The 1 H-NMR spectrum and infrared absorption spectrum were similar to those of polymer A.

[0130] Example 6 A mixed solution was obtained by slowly adding 1 mol of a diamine consisting of 7 mol % of n-nonanediamine and 93 mol % of 2-methyl-1,8-octanediamine to 200 mL of an ethanol solution containing 1 mol (13 g) of itaconic acid over a period of 2 hours at a liquid temperature of 45° C. while stirring.

[0131] The mixture solution obtained above was cooled to 25° C. to precipitate a white solid reaction product (yield: 96% by mass). The mixture solution was filtered to collect the reaction product, which was washed with ethanol at about 10° C. and then dried in a vacuum dryer at 45° C. for 12 hours.

[0132] Next, 20 g of the reaction product obtained above was mixed with 0.2 g of sodium dihydrogen phosphate as a catalyst, and the resulting mixture was heated to 190°C under reduced pressure to polymerize the reaction product for 6 hours, thereby obtaining a polyamide-based polymer.

[0133] The polyamide-based polymer obtained above was dissolved in N,N-dimethylformamide, and the resulting solution was added to acetone to purify the polyamide-based polymer. The polyamide-based polymer was then washed with acetone and dried in a vacuum dryer at 120°C for approximately 24 hours to obtain a purified polyamide-based polymer (hereinafter referred to as Polymer F) (yield: 92% by mass).

[0134] The number average molecular weight of the polymer F obtained above was 49,600. 1 The 1 H-NMR spectrum and infrared absorption spectrum were similar to those of polymer A.

[0135] Example 7 A mixed solution was obtained by slowly adding 1 mol of a diamine consisting of 6 mol % of n-nonanediamine and 94 mol % of 2-methyl-1,8-octanediamine to 200 mL of an ethanol solution containing 1 mol (13 g) of itaconic acid over a period of 2 hours at a liquid temperature of 45° C. while stirring.

[0136] The mixture solution obtained above was cooled to 25° C. to precipitate a white solid reaction product (yield: 96% by mass). The mixture solution was filtered to collect the reaction product, which was washed with ethanol at about 10° C. and then dried in a vacuum dryer at 45° C. for 12 hours.

[0137] Next, 20 g of the reaction product obtained above was mixed with 0.2 g of sodium dihydrogen phosphate as a catalyst, and the resulting mixture was heated to 190°C under reduced pressure to polymerize the reaction product for 6 hours, thereby obtaining a polyamide-based polymer.

[0138] The polyamide-based polymer obtained above was dissolved in N,N-dimethylformamide, and the resulting solution was added to acetone to purify the polyamide-based polymer. The polyamide-based polymer was then washed with acetone and dried in a vacuum dryer at 120°C for about 24 hours to obtain a purified polyamide-based polymer (hereinafter referred to as polymer G) (yield: 92% by mass). 1 The H-NMR spectrum is shown in Figure 5. The infrared absorption spectrum of polymer G was similar to that of polymer A.

[0139] Example 8 A mixed solution was obtained by slowly adding 1 mol of a diamine consisting of 96 mol % of n-nonanediamine and 4 mol % of 2-methyl-1,8-octanediamine to 200 mL of an ethanol solution containing 1 mol (13 g) of itaconic acid over a period of 2 hours at a liquid temperature of 45° C. while stirring.

[0140] The mixture solution obtained above was cooled to 25° C. to precipitate a white solid reaction product (yield: 96% by mass). The mixture solution was filtered to collect the reaction product, which was washed with ethanol at about 10° C. and then dried in a vacuum dryer at 45° C. for 12 hours.

[0141] Next, 20 g of the reaction product obtained above was mixed with 0.2 g of sodium dihydrogen phosphate as a catalyst, and the resulting mixture was heated to 190°C under reduced pressure to polymerize the reaction product for 6 hours, thereby obtaining a polyamide-based polymer.

[0142] The polyamide-based polymer obtained above was dissolved in N,N-dimethylformamide, and the resulting solution was added to acetone to purify the polyamide-based polymer. The polyamide-based polymer was then washed with acetone and dried in a vacuum dryer at 120°C for about 24 hours to obtain a purified polyamide-based polymer (hereinafter referred to as polymer H) (yield: 92% by mass). The nuclear magnetic resonance ( 1 The 1 H-NMR spectrum is shown in Figure 6. The nuclear magnetic resonance infrared absorption spectrum of polymer H was similar to that of polymer A.

[0143] Comparative Example 1 To 200 mL of an ethanol solution containing 1 mol (13 g) of itaconic acid, 1 mol of 1,6-hexamethylenediamine was slowly added over 2 hours with stirring while maintaining the liquid temperature of the ethanol solution at 45° C., thereby obtaining a mixed solution.

[0144] A white solid reaction product was precipitated by cooling the mixed solution obtained above to 25° C. The reaction product was collected by filtering the mixed solution, washed with ethanol at about 10° C., and then dried in a vacuum dryer at 45° C. for 12 hours.

[0145] Next, 20 g of the reaction product obtained above was mixed with 0.2 g of sodium dihydrogen phosphate as a catalyst, and the resulting mixture was heated to 190°C under reduced pressure to polymerize the reaction product for 6 hours, thereby obtaining a polyamide-based polymer.

[0146] The polyamide-based polymer obtained above was dissolved in N,N-dimethylformamide, and the resulting solution was added to acetone to purify the polyamide-based polymer. The polyamide-based polymer was then washed with acetone and dried in a vacuum dryer at 120°C for approximately 24 hours to obtain a purified polyamide-based polymer (yield: 89% by mass).

[0147] The Young's modulus of the polyamide-based polymer obtained above was measured as a physical property, and was found to be 580 MPa. This shows that the polyamide-based polymer has the same extensibility as polyethylene, fluororesin, etc., and is therefore not suitable for use as engineering plastics, etc.

[0148] The polyamide-based polymer obtained above was placed in a petri dish and immersed in water at 25°C. The polyamide-based polymer was then irradiated with light of 250 to 450 nm wavelengths from a high-pressure mercury lamp at 150 mW / cm. 2 When the polyamide-based polymer was irradiated with light of an intensity of 1000 nm, the polyamide-based polymer was completely dissolved in water about 6 hours after the light irradiation. This shows that the polyamide-based polymer has poor water resistance and is therefore not suitable for use in underwater applications such as fishing lines and fishing nets.

[0149] Next, the physical properties of the polymers A to F obtained above were examined, including the 10% weight loss temperature, the glass transition temperature, the tensile strength, and the Young's modulus. The results are shown in Table 1.

[0150] [Table 1]

[0151] From the results shown in Table 1, it can be seen that the polyamide polymers obtained in each Example all have excellent heat resistance since their 10% weight loss temperatures are 400°C or higher, their glass transition temperatures are 53 to 62°C, which are equivalent to or higher than the glass transition temperatures (about 50°C) of nylon 6 (polyamide 6) and nylon 66 (polyamide 66), and therefore have excellent heat resistance, and their Young's modulus is significantly higher than that of nylon 6 (polyamide 6) (about 1100 MPa) and that of nylon 66 (polyamide 66) (about 1500 MPa), and therefore these polymers are suitable for applications requiring stress.

[0152] Furthermore, among the polyamide-based polymers obtained in each Example, it is found that the tensile strength and Young's modulus of the polyamide-based polymer are synergistically improved when the molar ratio of the diamine that gives the repeating unit represented by formula (IIIa) to the diamine that gives the repeating unit represented by formula (IIIb) [diamine that gives the repeating unit represented by formula (IIIa) / diamine that gives the repeating unit represented by formula (IIIb)] is in the range of 20 / 80 to 80 / 20.

[0153] Next, the solubility of 1 mg of the polyamide-based polymer obtained in each Example in 1 mL of an organic solvent at 50° C. was examined. As a result, it was confirmed that the polyamide-based polymer obtained in each Example was soluble in organic solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, trifluoroacetic acid, and dimethyl sulfoxide.

[0154] This shows that the solution obtained by dissolving the polyamide-based polymer of the present invention in an organic solvent can be used as a spinning solution.

[0155] Next, 1 mg of the polyamide-based polymer obtained above was dissolved in 1 mL of each of the above organic solvents at 50° C. to obtain a solution, which was used as a spinning solution. The spinning solution was attached to a glass plate, a glass rod was brought into contact with the surface, and the glass rod was then removed from the glass plate. As a result, the spinning solution was stretched to 1 m or more, and filaments were formed. This confirmed that fibers could be easily produced using the spinning solution.

[0156] The polyamide-based polymers obtained above were each heated to 80° C., and the molten product was used as a molten spinning solution. The molten spinning solution obtained above was attached to a glass plate, a glass rod was brought into contact with the surface, and the glass rod was then removed from the glass plate. As a result, the molten spinning solution was stretched to 1 m or more and filaments were formed, confirming that fibers can be easily produced using the molten spinning solution.

[0157] Example 9 A mixed solvent of 20 mass % dioxane, 70 mass % N,N-dimethylformamide, and 10 mass % water was used as the solvent. 1 mole of diamine consisting of 78 mol % n-nonanediamine and 22 mol % 2-methyl-1,8-octanediamine was slowly added over 2 hours to 200 mL of a mixture containing 0.16 mol of itaconic acid and 0.84 mol of terephthalic acid at a liquid temperature of 80° C. under stirring to obtain a mixed solution.

[0158] The reaction product was precipitated as a white powder by cooling the mixed solution obtained above to 25° C. The reaction product was collected by filtering the mixed solution, washed with ethanol at about 10° C., and then dried in a vacuum dryer at 45° C. for 12 hours.

[0159] Next, 20 g of the reaction product obtained above was mixed with 0.2 g of sodium dihydrogen phosphate as a catalyst, and the resulting mixture was heated to 240°C under reduced pressure to polymerize the reaction product for 2 hours to obtain a polyamide-based polymer.

[0160] The polyamide-based polymer obtained above was added to a mixed solvent of 5% by mass of dimethyl sulfoxide and 95% by mass of isopropanol, and the resulting mixture was added to acetone to wash the polyamide-based polymer, and then the polyamide-based polymer was dried in a vacuum dryer at a temperature of 120° C. for about 24 hours to obtain a purified polyamide-based polymer (hereinafter referred to as polymer P). The number average molecular weight of the polymer P obtained above was 100,000.

[0161] Example 10 A mixed solvent of 20 mass % dioxane, 70 mass % N,N-dimethylformamide, and 10 mass % water was used as the solvent. 1 mole of a diamine consisting of 79 mol % n-nonanediamine and 21 mol % 2-methyl-1,8-octanediamine was slowly added over 2 hours to 200 mL of a mixture containing 0.28 mol of itaconic acid and 0.72 mol of terephthalic acid at a liquid temperature of 80° C. under stirring to obtain a mixed solution.

[0162] The reaction product was precipitated as a white powder by cooling the mixed solution obtained above to 25° C. The reaction product was collected by filtering the mixed solution, washed with ethanol at about 10° C., and then dried in a vacuum dryer at 45° C. for 12 hours.

[0163] Next, 20 g of the reaction product obtained above was mixed with 0.2 g of sodium dihydrogen phosphate as a catalyst, and the resulting mixture was heated to 240°C under reduced pressure to polymerize the reaction product for 2 hours to obtain a polyamide-based polymer.

[0164] The polyamide-based polymer obtained above was added to a mixed solvent of 5% by mass of dimethyl sulfoxide and 95% by mass of isopropanol, and the resulting mixture was added to acetone to wash the polyamide-based polymer, and then dried in a vacuum dryer at a temperature of 120° C. for about 24 hours to obtain a purified polyamide-based polymer (hereinafter referred to as Polymer Q). The number average molecular weight of the obtained Polymer Q was 100,000.

[0165] Example 11 A mixed solvent of 20 mass % dioxane, 70 mass % N,N-dimethylformamide, and 10 mass % water was used as the solvent. 1 mole of diamine consisting of 63 mol % n-nonanediamine and 37 mol % 2-methyl-1,8-octanediamine was slowly added over 2 hours to 200 mL of a mixture containing 0.42 mol of itaconic acid and 0.58 mol of terephthalic acid at a liquid temperature of 80° C. under stirring to obtain a mixed solution.

[0166] The reaction product was precipitated as a white powder by cooling the mixed solution obtained above to 25° C. The reaction product was collected by filtering the mixed solution, washed with ethanol at about 10° C., and then dried in a vacuum dryer at 45° C. for 12 hours.

[0167] Next, 20 g of the reaction product obtained above was mixed with 0.2 g of sodium dihydrogen phosphate as a catalyst, and the resulting mixture was heated to 240°C under reduced pressure to polymerize the reaction product for 2 hours to obtain a polyamide-based polymer.

[0168] The polyamide-based polymer obtained above was added to a mixed solvent of 5% by mass of dimethyl sulfoxide and 95% by mass of isopropanol, and the resulting mixture was added to acetone to wash the polyamide-based polymer, and then dried in a vacuum dryer at a temperature of 120° C. for about 24 hours to obtain a purified polyamide-based polymer (hereinafter referred to as Polymer R). The number average molecular weight of the obtained Polymer R was 100,000.

[0169] Example 12 A mixed solvent of 20 mass % dioxane, 70 mass % N,N-dimethylformamide, and 10 mass % water was used as the solvent. 1 mole of diamine consisting of 63 mol % n-nonanediamine and 37 mol % 2-methyl-1,8-octanediamine was slowly added over 2 hours to 200 mL of a mixture containing 0.56 mol of itaconic acid and 0.44 mol of terephthalic acid at a liquid temperature of 80° C. under stirring to obtain a mixed solution.

[0170] The reaction product was precipitated as a white powder by cooling the mixed solution obtained above to 25° C. The reaction product was collected by filtering the mixed solution, washed with ethanol at about 10° C., and then dried in a vacuum dryer at 45° C. for 12 hours.

[0171] Next, 20 g of the reaction product obtained above was mixed with 0.2 g of sodium dihydrogen phosphate as a catalyst, and the resulting mixture was heated to 240°C under reduced pressure to polymerize the reaction product for 2 hours to obtain a polyamide-based polymer.

[0172] The polyamide-based polymer obtained above was added to a mixed solvent of 5% by mass of dimethyl sulfoxide and 95% by mass of isopropanol, and the resulting mixture was added to acetone to wash the polyamide-based polymer. The resulting mixture was dried in a vacuum dryer at a temperature of 120°C for about 24 hours to obtain a purified polyamide-based polymer (hereinafter referred to as polymer S). The number average molecular weight of the polymer S obtained above was 100,000. The nuclear magnetic resonance ( 1 The H-NMR spectrum is shown in Figure 7. In Figure 7, Aromatic- means aromatic ring, and DMSO is a nuclear magnetic resonance ( 1 The term refers to the solvent dimethyl sulfoxide used in measuring the H-NMR spectrum.

[0173] Example 13 A mixed solvent of 20 mass % dioxane, 70 mass % N,N-dimethylformamide, and 10 mass % water was used as the solvent. 1 mole of a diamine consisting of 79 mol % n-nonanediamine and 21 mol % 2-methyl-1,8-octanediamine was slowly added over 2 hours to 200 mL of a mixture containing 0.77 mol of itaconic acid and 0.23 mol of terephthalic acid at a liquid temperature of 80° C. under stirring to obtain a mixed solution.

[0174] The reaction product was precipitated as a white powder by cooling the mixed solution obtained above to 25° C. The reaction product was collected by filtering the mixed solution, washed with ethanol at about 10° C., and then dried in a vacuum dryer at 45° C. for 12 hours.

[0175] Next, 20 g of the reaction product obtained above was mixed with 0.2 g of sodium dihydrogen phosphate as a catalyst, and the resulting mixture was heated to 240°C under reduced pressure to polymerize the reaction product for 2 hours to obtain a polyamide-based polymer.

[0176] The polyamide-based polymer obtained above was added to a mixed solvent of 5% by mass of dimethyl sulfoxide and 95% by mass of isopropanol, and the resulting mixture was added to acetone to wash the polyamide-based polymer, and then dried in a vacuum dryer at a temperature of 120° C. for about 24 hours to obtain a purified polyamide-based polymer (hereinafter referred to as polymer T). The number average molecular weight of the obtained polymer T was 100,000.

[0177] Example 14 A mixed solvent of 20 mass % dioxane, 70 mass % N,N-dimethylformamide, and 10 mass % water was used as the solvent. 1 mole of a diamine consisting of 20 mol % n-nonanediamine and 80 mol % 2-methyl-1,8-octanediamine was slowly added over 2 hours to 200 mL of a mixture containing 0.20 mol of itaconic acid and 0.80 mol of terephthalic acid at a liquid temperature of 80° C. under stirring to obtain a mixed solution.

[0178] The reaction product was precipitated as a white powder by cooling the mixed solution obtained above to 25° C. The reaction product was collected by filtering the mixed solution, washed with ethanol at about 10° C., and then dried in a vacuum dryer at 45° C. for 12 hours.

[0179] Next, 20 g of the reaction product obtained above was mixed with 0.2 g of sodium dihydrogen phosphate as a catalyst, and the resulting mixture was heated to 240°C under reduced pressure to polymerize the reaction product for 2 hours to obtain a polyamide-based polymer.

[0180] The polyamide-based polymer obtained above was added to a mixed solvent of 5% by mass of dimethyl sulfoxide and 95% by mass of isopropanol, and the resulting mixture was added to acetone to wash the polyamide-based polymer. The polyamide-based polymer was then dried in a vacuum dryer at a temperature of 120°C for about 24 hours to obtain a purified polyamide-based polymer (hereinafter referred to as polymer U). The number average molecular weight of the polymer U obtained above was 100,000. The infrared absorption spectrum of the polymer U obtained above is shown in Figure 8.

[0181] Next, the physical properties of the polymers P to T obtained above were examined, including the 10% weight loss temperature, glass transition temperature, melting point, tensile strength, and Young's modulus. The results are shown in Table 1.

[0182] [Table 2]

[0183] From the results shown in Table 2, it can be seen that the polyamide-based polymers obtained in each Example have excellent heat resistance since their 10% weight loss temperatures are 400°C or higher, their glass transition temperatures are 54 to 105°C, which are higher than the glass transition temperatures (approximately 50°C) of nylon 6 (polyamide 6) and nylon 66 (polyamide 66), and therefore have excellent heat resistance, and their Young's modulus is significantly higher than that of nylon 6 (polyamide 6) (approximately 1100 MPa) and that of nylon 66 (polyamide 66) (approximately 1500 MPa), making them suitable for applications requiring tension.

[0184] The polyamide-based polymers obtained above were each heated to 270°C, and the molten material was used as a molten spinning solution. The molten spinning solution obtained above was attached to a glass plate, a glass rod was brought into contact with the surface, and the glass rod was then removed from the glass plate. As a result, the molten spinning solution was stretched to 1m or more and filaments were formed, confirming that fibers could be easily produced using the molten spinning solution.

[0185] Next, the polymers P to T obtained above were placed in a petri dish, and while each was immersed in water at 25°C, light with wavelengths of 250 to 450 nm was irradiated onto the polymers P to T from a high-pressure mercury lamp at a rate of 150 mW / cm. 2 An accelerated light resistance test was conducted on polymers P to T, irradiating them with light at an intensity of 100 nm. As a result, it was confirmed that the diameter of each of polymers P to T had expanded to more than twice its original size 36 hours after the start of the light exposure. This shows that polymers P to T are hydrated and gradually decomposed when irradiated with light, and therefore have appropriate water resistance as well as decomposability and durability in water.

[0186] Next, the polymer D and polymer S obtained above were placed in a petri dish, and while immersed in water at 25°C, polymer D and polymer S were irradiated with light of 250 to 450 nm wavelengths at 150 mW / cm from a high-pressure mercury lamp. 2 Polymer D and Polymer S were exposed to irradiation at an intensity of 100 nm to perform an accelerated light resistance test.

[0187] In addition, polymer X consisting of 50 mol % itaconic acid and m-xylylenediamine and polymer Y consisting of 50 mol % itaconic acid and 50 mol % hexamethylenediamine were used as conventional polyamide-based polymers, and accelerated light resistance tests were also carried out on these polymers in the same manner as described above.

[0188] The results of the accelerated light fastness test are shown in Figure 9. In Figure 9, D indicates the result of the accelerated light fastness test of polymer D, S indicates the result of the accelerated light fastness test of polymer S, X indicates the result of the accelerated light fastness test of polymer X, and Y indicates the result of the accelerated light fastness test of polymer Y.

[0189] 9, it can be seen that polymers X and Y swelled in a short time and therefore had poor water resistance, whereas polymer D had excellent water resistance over a long period of time, and polymer S had excellent water resistance because it was less likely to swell than polymers X and Y, and all of the polymers had moderate water resistance as well as degradability and durability in water. Furthermore, since polymer S swelled in a shorter time than polymer D, it can be seen that the water resistance of the polyamide-based polymer of the present invention can be adjusted by adjusting the content of terephthalic acid in the polyamide-based polymer of the present invention. [Industrial Applicability]

[0190] The polyamide-based polymer of the present invention has appropriate water resistance, as well as degradability and durability in water, and has mechanical strength comparable to that of nylon. Therefore, it can be used as a replacement for conventional nylon in fishing equipment such as fishing nets and fishing lines, agricultural tools, and the like. Since it can also be used as a high-performance polyamide-based polymer, it is expected that when it is applied to automobile parts, it will contribute to reducing the weight of automobiles and thereby improving fuel efficiency.

[0191] In addition, the polyamide-based polymer of the present invention has appropriate water resistance, is degradable in water, is durable, and has excellent mechanical strength, and therefore is likely to be used in applications such as fibers such as sutures used in surgery on humans and other animals. Since the polyamide-based polymer of the present invention has the property of degrading in the presence of moisture, it is expected to be used in applications such as toys that are safe to eat.

Claims

1. A polyamide-based polymer obtained by polymerizing a dicarboxylic acid and a diamine, wherein the dicarboxylic acid is itaconic acid and the diamine is a compound represented by the formula (I): H 2 N-R 1 -NH 2 (I) (In the formula, R 1 represents a linear alkylene group having 8 to 10 carbon atoms. and a diamine represented by formula (II): H 2 N-R 2 -NH 2 (II) (In the formula, R 2 represents an alkylene group having 8 to 10 carbon atoms and having an alkyl group having 1 to 4 carbon atoms as a branched chain. The diamine represented by the formula (IIIa): 【Chemistry 1】 (wherein p represents an integer of 8 to 10). and a repeating unit represented by formula (IIIb): 【Chemistry 2】 (In the formula, R 2 is the same as above) and a repeating unit represented by the formula:

2. 2. The polyamide polymer according to claim 1, wherein the molar ratio of the diamine represented by formula (I) to the diamine represented by formula (II) [diamine represented by formula (I) / diamine represented by formula (II)] is 5 / 95 to 95 / 5.

3. A polyamide fiber comprising the polyamide polymer according to claim 1 or 2.

4. A molding material comprising the polyamide polymer according to claim 1 or 2.

Citation Information

Patent Citations

  • Automatic paper feed supplier in paper feeder of top feeder type

    JP1982077134A

  • Polyamide resin

    JP1995228689A

  • Cosmetic composition containing polyamide

    JP1997227356A

  • Method of producing polyamide

    JP2012107122A

  • Polyamide resin, a method for preparing the same, and an article comprising the same