Building material binders

A polyvinyl alcohol-based binder enhances the strength and durability of building materials, addressing their brittleness and impact resistance issues while utilizing waste materials.

JP7593621B2Active Publication Date: 2024-12-03WELOVE HLDG CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2021000674
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-01-06
Publication Date
2024-12-03
Estimated Expiration
2041-01-06

AI Technical Summary

Technical Problem

Existing building materials, such as gypsum boards, suffer from low impact resistance, poor bending resistance, and high brittleness, and materials using recycled waste materials have weak adhesive strength and brittleness.

Method used

A binder for building materials comprising a polyvinyl alcohol aqueous solution and polyvinyl alcohol resin powder, with specific concentration and polymerization ranges, is used to enhance the properties of building materials, including crosslinked polyvinyl alcohol powder for improved adhesion and strength.

Benefits of technology

The binder significantly increases impact strength, bending resistance, and reduces brittleness in building materials, allowing for the effective use of waste materials like sawdust and rice husks, and provides a suitable alternative to conventional gypsum boards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007593621000001
    Figure 0007593621000001
Patent Text Reader

Abstract

To provide building materials having high impact strength, excellent bending resistance and low brittleness, and compositions for building materials which can be suitably used for the building materials, and binders for the building materials which can be suitably used for the composition for the building materials.SOLUTION: A binder used for building materials contains a polyvinyl alcohol aqueous solution having a polyvinyl alcohol concentration of 5 to 20 mass% and a polyvinyl alcohol-based resin powder.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a binder for building materials. More specifically, the present invention relates to a binder for building materials that can improve the strength of building materials made of gypsum or the like and enables the effective use of sawdust, rice husks, and the like that are treated as waste, a composition for building materials that uses the binder for building materials, and a building material molded from the composition for building materials. [Background technology]

[0002] Generally, gypsum boards are manufactured by drying gypsum slurry on gypsum board base paper into a plate shape. Gypsum boards generally have the disadvantages of low impact strength, poor bending resistance, and high brittleness, since screws may spin when fastening fixtures, etc., to the gypsum board.

[0003] As a gypsum board capable of preventing the occurrence of warping, a gypsum board obtained by hardening a slurry containing calcined gypsum and cement has been proposed (see, for example, Patent Document 1). However, the gypsum board has the drawback of having low impact resistance and high brittleness because the calcined gypsum is solidified by cement.

[0004] Also, as a building material using recycled materials, a building material has been proposed in which ceramic waste, sawdust, leaf waste, waste wood, organic combustible materials such as resins, ceramic hardeners, glass-based binders and water are mixed and stirred to form a uniform viscous material, the viscous material is placed in a building material mold to form a base building material, the base building material is dried, heated to a temperature of 600 to 1000°C, the organic combustible materials are fired, and then allowed to cool naturally (see, for example, Patent Document 2). However, the building material has the disadvantage that the ceramic waste, organic combustible materials, etc. are bonded by a glass-based binder, so that the adhesive strength of these materials is weak, impact resistance is poor, and brittleness is high.

[0005] Therefore, in recent years, there has been a demand for the development of building materials that have high impact resistance, excellent bending resistance, and low brittleness. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] International Publication No. 2011 / 052048 Brochure [Patent Document 2] JP 2013-227188 A Summary of the Invention [Problem to be solved by the invention]

[0007] The present invention has been made in view of the above-mentioned conventional techniques, and an object of the present invention is to provide a building material having high impact resistance, excellent bending resistance, and low brittleness, a building material composition that can be suitably used for the building material, and a building material binder that can be suitably used for the building material composition. [Means for solving the problem]

[0008] The present invention relates to (1) A binder for use in building materials, which contains an aqueous polyvinyl alcohol solution having a polyvinyl alcohol concentration of 5 to 20% by mass and a polyvinyl alcohol-based resin powder. The content of the polyvinyl alcohol-based resin powder in the binder for building materials is 10 to 45 mass %, and a crosslinked polyvinyl alcohol powder is used as the polyvinyl alcohol-based resin powder. A binder for building materials, (2 ) The two-component binder is used for the material, and has an A component containing a polyvinyl alcohol aqueous solution having a polyvinyl alcohol concentration of 5 to 20 mass %, and a B component containing a polyvinyl alcohol resin powder. The amount of the polyvinyl alcohol-based resin powder per 100 parts by mass of the polyvinyl alcohol aqueous solution is 10 to 85 parts by mass, and a crosslinked polyvinyl alcohol powder is used as the polyvinyl alcohol-based resin powder. A two-component binder for building materials characterized by 、 (3 ) a composition for building materials, comprising the binder for building materials and a filler according to (1) or (2) above; and ( 4 ) The above ( 3A building material formed from the composition for building materials according to Regarding. Effect of the Invention

[0009] According to the present invention, there are provided a building material having high impact resistance, excellent bending resistance and low brittleness, a building material composition that can be suitably used for the building material, and a building material binder that can be suitably used for the building material composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] (1) Polyvinyl alcohol aqueous solution The polyvinyl alcohol aqueous solution can be easily prepared by dissolving polyvinyl alcohol in water to a predetermined concentration. Examples of water include pure water, purified water, ion-exchanged water, and tap water, but the present invention is not limited to these examples. The water may be at room temperature, heated, or cooled. The water may contain a water-soluble organic solvent within a range that does not impair the object of the present invention. Examples of water-soluble organic solvents include lower alcohols such as methyl alcohol, ethyl alcohol, n-propyl alcohol, isopropyl alcohol, n-butyl alcohol, and tert-butyl alcohol; polyhydric alcohols or monoesters thereof such as ethylene glycol, ethylene glycol monomethyl ether, ethylene glycol monobutyl ether, and diethylene glycol; and ketones such as acetone and methyl ethyl ketone, but the present invention is not limited to these examples. These water-soluble organic solvents may be used alone or in combination of two or more.

[0011] The average degree of polymerization of the polyvinyl alcohol used in the aqueous polyvinyl alcohol solution is preferably 300 or more, more preferably 500 or more, and even more preferably 1000 or more, from the viewpoint of increasing the impact resistance and improving the bending resistance of the building material by the binder for building materials of the present invention, and is preferably 4000 or less, more preferably 3000 or less, and even more preferably 2500 or less, from the viewpoint of improving the brittleness of the building material.

[0012] In the present invention, the average degree of polymerization of polyvinyl alcohol means the average degree of polymerization determined by a viscosity method.

[0013] The saponification degree of polyvinyl alcohol is preferably 90 mol% or more, more preferably 95 mol% or more, and even more preferably 98 mol% or more, from the viewpoint of increasing the impact resistance strength of the building material, improving the bending resistance, and improving the brittleness by the binder for building materials of the present invention. There is no upper limit for the saponification degree of polyvinyl alcohol, and the higher the degree, the more preferable it is, and completely saponified polyvinyl alcohol is preferred.

[0014] The concentration of polyvinyl alcohol in the aqueous polyvinyl alcohol solution is 5% by mass or more, preferably 8% by mass or more, from the viewpoint of increasing the impact strength, improving the bending resistance, and improving brittleness of the building material by the binder for building materials of the present invention, and is 20% by mass or less, preferably 15% by mass or less, from the viewpoint of increasing the impact strength, improving the bending resistance, and improving brittleness of the building material.

[0015] (2) Polyvinyl alcohol resin powder From the viewpoint of increasing the impact strength, improving the bending resistance, and improving the brittleness of the building material, the polyvinyl alcohol-based resin powder is preferably at least one type of polyvinyl alcohol-based resin powder selected from the group consisting of polyvinyl alcohol powder and crosslinked polyvinyl alcohol powder. The polyvinyl alcohol powder and the crosslinked polyvinyl alcohol powder may be used alone or in combination.

[0016] One of the features of the present invention is that the polyvinyl alcohol-based resin powder is used. By using the polyvinyl alcohol-based resin powder in combination with an aqueous polyvinyl alcohol solution, it is possible to increase the impact resistance of the building material, improve its bending resistance, and reduce its brittleness.

[0017] The reason why the binder for building materials of the present invention exhibits such excellent effects is not clear, but it is believed that this is due to the fact that the binder for building materials of the present invention uses the polyvinyl alcohol-based resin powder and an aqueous polyvinyl alcohol solution in combination, and since polyvinyl alcohol is used in both the polyvinyl alcohol-based resin powder and the aqueous polyvinyl alcohol solution, the affinity between the aqueous polyvinyl alcohol solution and the polyvinyl alcohol-based resin powder is excellent, and the aqueous polyvinyl alcohol solution is interposed between the particles of the polyvinyl alcohol-based resin powder, and when water, which is the solvent contained in the binder for building materials, evaporates, the particles of the polyvinyl alcohol-based resin powder are bonded to each other via the polyvinyl alcohol contained in the aqueous polyvinyl alcohol solution, and the polyvinyl alcohol-based resin powder adheres firmly to the excipient used in the composition for building materials via the polyvinyl alcohol.

[0018] Among the polyvinyl alcohol-based resin powders, crosslinked polyvinyl alcohol powders are preferred from the viewpoints of increasing the impact strength, improving bending resistance, and improving brittleness of the building material.

[0019] The particle size of the polyvinyl alcohol-based resin powder is preferably 0.1 to 1 mm, and more preferably 0.3 to 0.6 mm, from the viewpoints of increasing the impact resistance strength, improving bending resistance, and improving brittleness of the building material.

[0020] The particle size of the polyvinyl alcohol-based resin powder means the opening of a JIS mesh (sieve). Therefore, the lower limit of the particle size of the polyvinyl alcohol-based resin powder means the opening when the polyvinyl alcohol-based resin powder is present on a sieve having a specific opening, and the upper limit of the particle size of the polyvinyl alcohol-based resin powder means the opening when the polyvinyl alcohol-based resin powder passes through a sieve having a specific opening. For example, a polyvinyl alcohol-based resin powder having a particle size of 0.1 to 1 mm is a polyvinyl alcohol-based resin powder that is present on a sieve obtained by passing coarse particles of the polyvinyl alcohol-based resin powder through a JIS sieve having a 16 mesh opening (under mesh) and then passing the polyvinyl alcohol-based resin powder through the sieve through a JIS sieve having a 149 mesh opening (over mesh) with a 0.1 mm opening.

[0021] The particle size of the polyvinyl alcohol-based resin powder can be easily adjusted using a sieve (JIS mesh).

[0022] For example, a polyvinyl alcohol-based resin powder having a particle size within a predetermined range may inevitably contain a polyvinyl alcohol-based resin powder having a particle size outside the predetermined range. In the present invention, a polyvinyl alcohol-based resin powder having a particle size outside the predetermined range may be contained within a range that does not impair the object of the present invention.

[0023] [Polyvinyl alcohol powder] Polyvinyl alcohol powder is usually commercially available as a powder or granules. Since polyvinyl alcohol powder is water-soluble, it is preferable to add the polyvinyl alcohol powder to an aqueous polyvinyl alcohol solution immediately before using the binder for building materials of the present invention, and prepare a binder for building materials in which the polyvinyl alcohol powder is dispersed in the aqueous polyvinyl alcohol solution.

[0024] Therefore, when polyvinyl alcohol powder is used as the polyvinyl alcohol-based resin powder, or when polyvinyl alcohol powder and cross-linked polyvinyl alcohol powder are used in combination, a two-component building material binder may be prepared in which component A containing an aqueous polyvinyl alcohol solution and component B containing a polyvinyl alcohol-based resin powder containing at least polyvinyl alcohol powder are separated, and when using the two-component building material binder, component A and component B may be mixed and used.

[0025] The average polymerization degree of polyvinyl alcohol used in the polyvinyl alcohol powder is preferably 300 or more, more preferably 500 or more, and even more preferably 1000 or more, from the viewpoint of increasing the impact strength and improving the bending resistance of the building material by the binder for building materials of the present invention, and is preferably 4000 or less, more preferably 3000 or less, and even more preferably 2500 or less, from the viewpoint of improving the brittleness of the building material. In addition, the saponification degree of the polyvinyl alcohol is preferably 90 mol% or more, more preferably 95 mol% or more, and even more preferably 98 mol% or more, from the viewpoint of increasing the impact strength, improving the bending resistance, and improving the brittleness of the building material by the binder for building materials of the present invention. There is no upper limit to the saponification degree of polyvinyl alcohol, and the higher the better, and fully saponified polyvinyl alcohol is preferred.

[0026] [Crosslinked polyvinyl alcohol powder] The crosslinked polyvinyl alcohol powder means a powder of polyvinyl alcohol having a crosslinked structure.

[0027] The average polymerization degree of polyvinyl alcohol used as a raw material for the crosslinked polyvinyl alcohol powder is preferably 300 or more, more preferably 500 or more, and even more preferably 1000 or more, from the viewpoint of increasing the impact strength and improving the bending resistance of the building material by the binder for building materials of the present invention, and is preferably 4000 or less, more preferably 3000 or less, and even more preferably 2500 or less, from the viewpoint of improving the brittleness of the building material. In addition, the saponification degree of the polyvinyl alcohol is preferably 90 mol% or more, more preferably 95 mol% or more, and even more preferably 98 mol% or more, from the viewpoint of increasing the impact strength, improving the bending resistance, and improving the brittleness of the building material by the binder for building materials of the present invention. There is no upper limit to the saponification degree of polyvinyl alcohol, and the higher the better, and fully saponified polyvinyl alcohol is preferred.

[0028] Crosslinked polyvinyl alcohol can be prepared by crosslinking polyvinyl alcohol. Examples of methods for preparing crosslinked polyvinyl alcohol include a method for preparing crosslinked polyvinyl alcohol by cooling and thawing an aqueous solution of polyvinyl alcohol, and a method for preparing crosslinked polyvinyl alcohol by crosslinking polyvinyl alcohol with a crosslinking agent, but the present invention is not limited to these examples.

[0029] [Cross-linking by cooling and thawing] When preparing crosslinked polyvinyl alcohol by cooling and thawing an aqueous solution of polyvinyl alcohol, the concentration of polyvinyl alcohol in the aqueous solution of polyvinyl alcohol is preferably 1 mass % or more, more preferably 3 mass % or more, and even more preferably 5 mass % or more, from the viewpoints of increasing the impact strength, improving bending resistance, and improving brittleness of the building material, and is preferably 40 mass % or less, more preferably 30 mass % or less, and even more preferably 20 mass % or less, from the viewpoint of improving the solubility of polyvinyl alcohol.

[0030] The aqueous solution of polyvinyl alcohol may contain water-soluble organic solvents, such as water-soluble compounds such as dimethyl sulfoxide; lower alcohols such as methyl alcohol, ethyl alcohol, n-propyl alcohol, isopropyl alcohol, n-butyl alcohol, and tert-butyl alcohol; polyhydric alcohols or monoesters thereof such as ethylene glycol, ethylene glycol monomethyl ether, ethylene glycol monobutyl ether, and diethylene glycol; and ketones such as acetone and methyl ethyl ketone, within the scope of the object of the present invention.

[0031] The polyvinyl alcohol aqueous solution can be thawed by, for example, placing a container filled with the polyvinyl alcohol aqueous solution in a freezer (room temperature: -10°C or lower), cooling for about 5 to 15 hours, removing it from the freezer, and leaving it at room temperature until it reaches room temperature. The polyvinyl alcohol aqueous solution may be thawed by cooling multiple times as necessary.

[0032] The crosslinked polyvinyl alcohol obtained by cooling and thawing the aqueous solution of polyvinyl alcohol as described above contains a solvent (water), so it is preferable to dry it. Methods for drying the crosslinked polyvinyl alcohol include, for example, reduced pressure drying, hot air drying, and heat drying, but the present invention is not limited to these examples.

[0033] When the dried crosslinked polyvinyl alcohol is in a lump form, the lump crosslinked polyvinyl alcohol can be pulverized and classified using a sieve to obtain a crosslinked polyvinyl alcohol powder having a predetermined particle size.

[0034] [Crosslinking with crosslinking agent] Crosslinked polyvinyl alcohol can be readily prepared by crosslinking polyvinyl alcohol with a crosslinking agent.

[0035] Examples of the crosslinking agent include boron compounds such as boric acid and / or boric acid salts (hereinafter also referred to as boric acid (salts)) typified by boric acid, potassium borate, sodium borate (borax), and other boric acid salts; titanium, titanium acetyl acetate, triethanolamine titanate, titanium ammonium lactate, titanium lactate, and other titanium and its compounds; zirconium, zirconium fluoride, zirconium chloride, zirconium bromide, zirconium sulfate, zirconium nitrate, zirconium carbonate, ammonium zirconium carbonate, potassium zirconium carbonate, zirconium acetate, zirconium stearate, Examples of the crosslinking agent include polyvalent metals and their compounds, such as zirconium octylate, zirconium citrate, zirconium lactate, zirconium phosphate, zirconic acid, zirconate salts, and other zirconium compounds; and amine compounds, such as ethylenediamine, hexamethylenediamine, diethylenetriamine, dipropylenetriamine, triethylenetetramine, tetraethylenepentamine, N-aminoethylpiperazine, 1,4-bis(3-aminopropyl)piperazine, trimethylhexamethylenediamine, and polyoxypropylenediamine, but the present invention is not limited to these examples. Each of these crosslinking agents may be used alone, or two or more types may be used in combination.

[0036] Among the crosslinking agents, boron compounds are preferred, and boric acid (salts) are more preferred, because they rapidly crosslink polyvinyl alcohol. Among the boric acid (salts), boric acid and borax are preferred, and borax is more preferred, because they increase the impact strength of the building material, improve bending resistance, and improve brittleness.

[0037] When the crosslinking agent is water-soluble, it can be used as an aqueous solution, and when the crosslinking agent is water-insoluble, it can be used as an aqueous dispersion. For example, when boric acid (salt) is used as the crosslinking agent, since boric acid (salt) is water-soluble, it can be dissolved in water to a predetermined concentration and used as an aqueous solution. Examples of water used in the aqueous solution and aqueous dispersion include pure water, purified water, ion-exchanged water, and tap water, but the present invention is not limited to only these examples. The water temperature may be room temperature, or the water may be heated or cooled. From the viewpoint of increasing the crosslinking efficiency, the amount of the crosslinking agent per 1 L (liter) of water is preferably 1 g or more, more preferably 5 g or more, and even more preferably 10 g or more, and the upper limit of the amount is not particularly limited, but is usually 100 g or less. The liquid temperature of the aqueous solution and aqueous dispersion is not particularly limited, but is usually preferably room temperature to about 40°C.

[0038] The amount of crosslinking agent per 100 parts by mass of polyvinyl alcohol varies depending on the average degree of polymerization of the polyvinyl alcohol and the type of the crosslinking agent, but from the viewpoint of sufficiently crosslinking the polyvinyl alcohol, it is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and even more preferably 5 parts by mass or more, and from the viewpoint of preventing unreacted crosslinking agent from remaining, it is preferably 60 parts by mass or less, more preferably 55 parts by mass or less, and even more preferably 50 parts by mass or less.

[0039] When polyvinyl alcohol comes into contact with a crosslinking agent, it crosslinks to produce crosslinked polyvinyl alcohol, which then gels. Therefore, crosslinked polyvinyl alcohol can be obtained by contacting polyvinyl alcohol with a crosslinking agent. When polyvinyl alcohol and a crosslinking agent are mixed, it is preferable to use both polyvinyl alcohol and the crosslinking agent as aqueous solutions in order to react them uniformly. The temperature at which polyvinyl alcohol and a crosslinking agent are mixed is not particularly limited, but is usually preferably room temperature to about 40°C in order to promote crosslinking of polyvinyl alcohol and increase production efficiency.

[0040] The crosslinked polyvinyl alcohol obtained by crosslinking polyvinyl alcohol as described above contains a solvent (water), so it is preferable to dry it. As a method for drying crosslinked polyvinyl alcohol, for example, reduced pressure drying method, hot air drying method, heat drying method, etc. can be mentioned, but the present invention is not limited to only these examples.

[0041] When the dried crosslinked polyvinyl alcohol is in a lump form, the lump crosslinked polyvinyl alcohol can be pulverized and classified using a sieve to obtain a crosslinked polyvinyl alcohol powder having a predetermined particle size.

[0042] When a cross-linked polyvinyl alcohol powder is used as the polyvinyl alcohol-based resin powder, a two-component building material binder may be prepared by separating component A containing an aqueous polyvinyl alcohol solution from component B containing a cross-linked polyvinyl alcohol powder, and the building material binder may be used by mixing component A and component B.

[0043] The crosslinked polyvinyl alcohol powder may contain other resin powders, inorganic powders, and other powders, and may also contain additives such as preservatives, antibacterial agents, antioxidants, and colorants, as long as the object of the present invention is not impaired.

[0044] (3) Binders for building materials The binder for building materials of the present invention is characterized by containing an aqueous polyvinyl alcohol solution having a polyvinyl alcohol concentration of 5 to 20 mass % and a polyvinyl alcohol-based resin powder.

[0045] Since the binder for building materials of the present invention contains the aqueous polyvinyl alcohol solution and the polyvinyl alcohol-based resin powder, it is possible to increase the impact resistance of building materials, improve their bending resistance, and reduce their brittleness.

[0046] The binder for building materials of the present invention can be easily prepared by mixing the aqueous polyvinyl alcohol solution and the polyvinyl alcohol-based resin powder.

[0047] The liquid temperature of the polyvinyl alcohol aqueous solution when mixing the polyvinyl alcohol aqueous solution and the polyvinyl alcohol resin powder is not particularly limited. When the polyvinyl alcohol resin powder contains polyvinyl alcohol powder, the liquid temperature is preferably 0 to 20°C, more preferably 1 to 15°C, and even more preferably 3 to 10°C, from the viewpoint of making the polyvinyl alcohol powder difficult to dissolve in the polyvinyl alcohol aqueous solution. When the polyvinyl alcohol resin powder does not contain polyvinyl alcohol powder but contains crosslinked polyvinyl alcohol powder, the liquid temperature of the polyvinyl alcohol aqueous solution is preferably 0 to 40°C, more preferably 1 to 35°C, and even more preferably 3 to 30°C, from the viewpoint of improving the handleability of the polyvinyl alcohol aqueous solution, and may be room temperature.

[0048] In addition, the liquid temperature of the binder for building materials obtained by mixing the polyvinyl alcohol aqueous solution with the polyvinyl alcohol-based resin powder is not particularly limited. When the polyvinyl alcohol-based resin powder contains polyvinyl alcohol powder, the liquid temperature is preferably 0 to 20°C, more preferably 1 to 15°C, and even more preferably 3 to 10°C, from the viewpoint of making the polyvinyl alcohol powder difficult to dissolve in the polyvinyl alcohol aqueous solution. In addition, when the polyvinyl alcohol-based resin powder does not contain polyvinyl alcohol powder but contains crosslinked polyvinyl alcohol powder, the liquid temperature of the polyvinyl alcohol aqueous solution is preferably 0 to 40°C, more preferably 1 to 35°C, and even more preferably 3 to 30°C, from the viewpoint of improving the handleability of the polyvinyl alcohol aqueous solution, and may be room temperature.

[0049] The content of the polyvinyl alcohol-based resin powder in the binder for building materials of the present invention varies slightly depending on the concentration of polyvinyl alcohol contained in the aqueous polyvinyl alcohol solution, but is preferably 5 to 50 mass %, more preferably 10 to 45 mass %, from the viewpoint of increasing the impact strength, improving bending resistance, and improving brittleness of the building material. Therefore, the content of the aqueous polyvinyl alcohol solution in the binder for building materials of the present invention varies slightly depending on the concentration of polyvinyl alcohol contained in the aqueous polyvinyl alcohol solution, but is preferably 50 to 95 mass %, more preferably 55 to 90 mass %, from the viewpoint of increasing the impact strength, improving bending resistance, and improving brittleness of the building material.

[0050] The binder for building materials of the present invention may contain additives such as preservatives, antibacterial agents, antioxidants, and colorants, if necessary, within the scope of not impairing the object of the present invention. These additives may be used alone or in combination of two or more. The content of the additives in the binder for building materials varies depending on the type of the additive, and therefore it is preferable to appropriately adjust the content depending on the type of the additive.

[0051] (4) Two-component building material binders The binder for building materials of the present invention can be used as a two-component binder for building materials having a component A containing an aqueous polyvinyl alcohol solution having a polyvinyl alcohol concentration of 5 to 20 mass % and a component B containing a polyvinyl alcohol-based resin powder.

[0052] When the binder for building materials of the present invention is a two-component binder for building materials, the binder for building materials can be obtained by mixing component A containing an aqueous polyvinyl alcohol solution and component B containing a polyvinyl alcohol-based resin powder to a uniform composition immediately before using the binder for building materials of the present invention. When the polyvinyl alcohol-based resin powder contains a polyvinyl alcohol powder, the polyvinyl alcohol powder can be prevented from dissolving in the aqueous polyvinyl alcohol solution, and when the polyvinyl alcohol-based resin powder contains a crosslinked polyvinyl alcohol powder, the crosslinked polyvinyl alcohol powder can be prevented from swelling in the aqueous polyvinyl alcohol solution.

[0053] When the binder for building materials of the present invention is used as a two-component binder for building materials, the amount of the aqueous polyvinyl alcohol solution and the amount of the polyvinyl alcohol-based resin powder in the finished state of the binder for two-component building materials are not particularly limited. When the binder for two-component building materials is actually used, the amount of the polyvinyl alcohol-based resin powder per 100 parts by mass of the aqueous polyvinyl alcohol solution varies slightly depending on the concentration of polyvinyl alcohol contained in the aqueous polyvinyl alcohol solution, but is preferably 5 to 100 parts by mass, more preferably 10 to 85 parts by mass, from the viewpoint of increasing the impact strength of the building material, improving the bending resistance, and improving the brittleness.

[0054] (5) Composition for building materials The binder for building materials of the present invention can be suitably used in a composition for building materials. The composition for building materials is used as a raw material for building materials. The building materials can be produced by molding the composition for building materials into a predetermined shape.

[0055] The building material composition of the present invention contains the building material binder and a filler. Examples of fillers include gypsum, sawdust, rice husk, shell powder, diatomaceous earth, and cement, but the present invention is not limited to these examples. These fillers may be used alone or in combination of two or more. Among these fillers, gypsum, sawdust, rice husk, shell powder, and diatomaceous earth are preferred.

[0056] Gypsum, the core material of gypsum boards, has excellent heat and fire resistance, but on the other hand, it has poor impact resistance and is brittle, so when screws are tightened to attach various components to the gypsum board, they may spin freely.

[0057] In contrast, even when the building material composition of the present invention uses gypsum as a filler, a board formed from the building material composition has increased impact resistance, improved bending resistance, and improved brittleness, compared to the gypsum used as the core material of conventional gypsum boards.

[0058] Therefore, when gypsum is used as a filler in the building material composition of the present invention, a board molded using the building material composition has higher impact resistance, excellent bending resistance, and improved brittleness compared to the gypsum used as the core material of conventional gypsum boards, and is therefore expected to be widely used as a substitute for conventional gypsum boards.

[0059] Conventionally, sawdust, rice husks, shells, etc. have been incinerated as waste or dumped in the ground.

[0060] In contrast, when vegetable waste such as sawdust and rice husks is used as the filler for the building material composition of the present invention, the building material board molded from the building material composition containing the vegetable waste has high impact strength, excellent bending resistance, and low brittleness, so it can be suitably used as a building material. Furthermore, when shells such as scallops are used as the filler for the building material composition of the present invention, the building material board molded from the building material composition containing the shells has high impact strength, excellent bending resistance, and low brittleness, like the vegetable waste, so it can be suitably used as a building material.

[0061] Therefore, the composition for building materials of the present invention exerts an excellent effect of enabling effective utilization of waste materials that have conventionally been discarded or incinerated.

[0062] The shape and size of the filler used in the building material composition of the present invention are not particularly limited, and it is preferable to adjust them appropriately depending on the application of the resulting building material. For example, when the filler is sawdust or rice husk, the sawdust and rice husk can be used as they are, or can be crushed according to the application. When the filler is shell, it can be crushed into powder.

[0063] In the composition for building materials of the present invention, the amount of the excipient per 100 parts by mass of the binder for building materials varies depending on the type of the excipient and the use of the resulting building material, so it cannot be determined in general, and it is preferable to appropriately determine the amount according to the type of the excipient and the use of the resulting building material. In order to increase the impact strength of the building material, improve the bending resistance, and improve the brittleness, the amount of the excipient per 100 parts by mass of the binder for building materials is generally preferably adjusted within a range of 100 to 450 parts by mass, more preferably 100 to 400 parts by mass, and even more preferably 100 to 350 parts by mass.

[0064] The composition for building materials of the present invention can be easily prepared by mixing the binder for building materials and the excipient to obtain a uniform composition. The composition for building materials thus obtained can be molded into a predetermined shape to obtain a building material.

[0065] (6) Building materials The building material of the present invention can be produced by molding the building material composition of the present invention by a molding method such as hot press molding, injection molding, blow molding, extrusion molding, etc. For example, when the building material is produced by molding the building material composition of the present invention by hot press molding, the building material composition can be filled into a mold having a predetermined shape, and the filling in the mold can be pressed from above with a heated mold to form the material.

[0066] The size and shape of the building material obtained as described above are arbitrary, and it is preferable to appropriately adjust them according to the application of the building material. When the building material of the present invention is used as a substitute for a gypsum board, the building material composition of the present invention can be molded into a plate having a thickness of, for example, 8 to 25 mm.

[0067] The building material of the present invention uses the building material binder of the present invention, and therefore has increased impact resistance, improved bending resistance, and improved brittleness compared to those not using the building material binder, and can therefore be suitably used, for example, as a building material for buildings such as residential buildings. EXAMPLES

[0068] Next, the binder for building materials of the present invention will be described in more detail based on examples, but the present invention is not limited to only these examples.

[0069] Manufacturing Example 1 Polyvinyl alcohol having an average degree of polymerization of 1700 and a degree of saponification of approximately 98 to 99 mol% (manufactured by Kuraray Co., Ltd., product name: Kuraray Poval PVA-117) was dissolved in water to a concentration of 3 mass%, to obtain an aqueous polyvinyl alcohol solution (hereinafter referred to as PVA solution A, and indicated as A in Table 1 below).

[0070] Manufacturing Example 2 Polyvinyl alcohol having an average degree of polymerization of 1700 and a degree of saponification of approximately 98 to 99 mol% (manufactured by Kuraray Co., Ltd., product name: Kuraray Poval PVA-117) was dissolved in water to a concentration of 5 mass%, to obtain an aqueous polyvinyl alcohol solution (hereinafter referred to as PVA solution B; indicated as B in Table 1 below).

[0071] Production Example 3 Polyvinyl alcohol having an average degree of polymerization of 1700 and a degree of saponification of approximately 98 to 99 mol% (manufactured by Kuraray Co., Ltd., product name: Kuraray Poval PVA-117) was dissolved in water to a concentration of 10 mass%, to obtain an aqueous polyvinyl alcohol solution (hereinafter referred to as PVA solution C; indicated as C in Table 1 below).

[0072] Production Example 4 Polyvinyl alcohol having an average degree of polymerization of 1700 and a degree of saponification of approximately 98 to 99 mol% (manufactured by Kuraray Co., Ltd., product name: Kuraray Poval PVA-117) was dissolved in water to a concentration of 15 mass%, to obtain an aqueous polyvinyl alcohol solution (hereinafter referred to as PVA solution D, and indicated as D in Table 1 below).

[0073] Production Example 5 Polyvinyl alcohol having an average degree of polymerization of 1700 and a degree of saponification of approximately 98 to 99 mol% (manufactured by Kuraray Co., Ltd., product name: Kuraray Poval PVA-117) was dissolved in water to a concentration of 20 mass%, to obtain an aqueous polyvinyl alcohol solution (hereinafter referred to as PVA solution E; indicated as E in Table 1 below).

[0074] Production Example 6 Polyvinyl alcohol having an average degree of polymerization of 500 and a degree of saponification of approximately 98 to 99 mol% (manufactured by Kuraray Co., Ltd., product name: Kuraray Poval PVA-105) was dissolved in water to a concentration of 15 mass%, to obtain an aqueous polyvinyl alcohol solution (hereinafter referred to as PVA solution F; indicated as F in Table 1 below).

[0075] Production Example 7 Polyvinyl alcohol having an average degree of polymerization of 2400 and a degree of saponification of approximately 98 to 99 mol% (manufactured by Kuraray Co., Ltd., product name: Kuraray Poval PVA-124) was dissolved in water to a concentration of 15 mass%, to obtain an aqueous polyvinyl alcohol solution (hereinafter referred to as PVA solution G, and indicated as G in Table 1 below).

[0076] Production Example 8 Polyvinyl alcohol having an average degree of polymerization of 2400 and a degree of saponification of approximately 98 to 99 mol% (manufactured by Kuraray Co., Ltd., product name: Kuraray Poval PVA-124) was dissolved in water to a concentration of 25 mass%, to obtain an aqueous polyvinyl alcohol solution (hereinafter referred to as PVA solution H; indicated as H in Table 1 below).

[0077] Preparation Example 1 Polyvinyl alcohol having an average degree of polymerization of 1700 and a degree of saponification of approximately 98 to 99 mol% (manufactured by Kuraray Co., Ltd., product name: Kuraray Poval PVA-117) was crushed in a mortar, and the crushed material obtained was classified using a JIS sieve with an opening of 300 μm and a JIS sieve with an opening of 600 μm to obtain a polyvinyl alcohol powder (hereinafter referred to as PVA powder A, and indicated as A in Table 1 below).

[0078] Preparation Example 2 Polyvinyl alcohol having an average degree of polymerization of 500 and a degree of saponification of approximately 98 to 99 mol% (manufactured by Kuraray Co., Ltd., product name: Kuraray Poval PVA-105) was crushed in a mortar, and the crushed material obtained was classified using a JIS sieve with an opening of 300 μm and a JIS sieve with an opening of 600 μm to obtain a polyvinyl alcohol powder (hereinafter referred to as PVA powder B, and indicated as B in Table 1 below).

[0079] Preparation Example 3 Polyvinyl alcohol having an average degree of polymerization of 2400 and a degree of saponification of approximately 98 to 99 mol% (manufactured by Kuraray Co., Ltd., product name: Kuraray Poval PVA-124) was crushed in a mortar, and the crushed material obtained was classified using a JIS sieve with an opening of 300 μm and a JIS sieve with an opening of 600 μm to obtain a polyvinyl alcohol powder (hereinafter referred to as PVA powder C, and indicated as C in Table 1 below).

[0080] Preparation Example 4 An aqueous solution (liquid temperature: 20°C) containing 10% by mass of polyvinyl alcohol (manufactured by Kuraray Co., Ltd., product name: Kuraray Poval PVA-117) having an average degree of polymerization of 1700 and a degree of saponification of approximately 98 to 99 mol% was poured into a rectangular polypropylene resin container having a length of 25 cm, a width of 20 cm, and a depth of 7 cm on the inner surface of the container to a depth of approximately 2 mm.The resin container was then placed in a freezer (room temperature: -20°C) and cooled for 5 hours.Then, the container was removed from the freezer and left at room temperature until it reached room temperature, thereby obtaining a sheet.

[0081] Next, the sheet obtained above was removed from the resin container, placed in a dryer, heated to 60°C, and held at the same temperature for 10 minutes, then removed from the dryer and allowed to cool to obtain a dried sheet. The sheet obtained above was crushed in a mortar, and the crushed material was classified using a JIS sieve with a mesh size of 300 μm and a JIS sieve with a mesh size of 600 μm to obtain a crosslinked polyvinyl alcohol powder (hereinafter referred to as PVA powder D, denoted as D in Table 1 below).

[0082] Preparation Example 5 An aqueous solution (liquid temperature: 20°C) containing 10% by mass of polyvinyl alcohol (manufactured by Kuraray Co., Ltd., product name: Kuraray Poval PVA-105) with an average degree of polymerization of 500 and a degree of saponification of approximately 98 to 99 mol% was poured into a rectangular polypropylene resin container with a length of 25 cm, a width of 20 cm, and a depth of 7 cm on the inner surface of the container to a depth of approximately 2 mm.The resin container was then placed in a freezer (room temperature: -20°C) and cooled for 5 hours.Then, the container was removed from the freezer and left at room temperature until it reached room temperature, thereby obtaining a sheet.

[0083] Next, the sheet obtained above was removed from the resin container, placed in a dryer, heated to 60°C, and held at the same temperature for 10 minutes, then removed from the dryer and allowed to cool to obtain a dried sheet. The sheet obtained above was crushed in a mortar, and the crushed material was classified using a JIS sieve with a mesh size of 300 μm and a JIS sieve with a mesh size of 600 μm to obtain a crosslinked polyvinyl alcohol powder (hereinafter referred to as PVA powder E, denoted as E in Table 1 below).

[0084] Preparation Example 6 An aqueous solution (liquid temperature: 20°C) containing 10% by mass of polyvinyl alcohol (manufactured by Kuraray Co., Ltd., product name: Kuraray Poval PVA-124) with an average degree of polymerization of 2400 and a degree of saponification of approximately 98 to 99 mol% was poured into a rectangular polypropylene resin container with a length of 25 cm, a width of 20 cm, and a height of 7 cm on the inner surface of the container to a depth of approximately 2 mm.The resin container was then placed in a freezer (room temperature: -20°C) and cooled for 5 hours, after which it was removed from the freezer and left at room temperature until it reached room temperature, thereby obtaining a sheet.

[0085] Next, the sheet obtained above was taken out of the resin container, placed in a dryer, heated to 60°C, and held at the same temperature for 10 minutes, then taken out of the dryer and allowed to cool to obtain a dried sheet. The sheet obtained above was crushed in a mortar, and the crushed material was classified using a JIS sieve with a mesh size of 300 μm and a JIS sieve with a mesh size of 600 μm to obtain a crosslinked polyvinyl alcohol powder (hereinafter referred to as PVA powder F, denoted as F in Table 1 below).

[0086] Examples 1 to 30 and Comparative Examples 1 to 8 The PVA solution obtained in each production example was used as component A, and the PVA powder obtained in each preparation example was used as component B. By combining components A and B, a two-component binder for building materials was obtained.

[0087] Next, the PVA solution used in the two-component binder for building materials obtained above was mixed with PVA powder to obtain a binder for building materials having the PVA powder content shown in Table 1.

[0088] A building material composition was obtained by mixing the building material binder and the excipient in the amount shown in Table 1 with respect to 100 parts by mass of the building material binder obtained above to obtain a uniform composition.

[0089] The symbols in the "Type and amount of excipient" column in Table 1 refer to the following excipients. P: Gypsum (manufactured by Yoshino Gypsum Sales Co., Ltd., product name: Histone N) Q: Sawdust (made by Shimada Kowari Manufacturing Co., Ltd., cedar sawdust) R: Rice husks (rice husks from Koshihikari rice produced in Shiga Prefecture) S: Shell powder [OH Lab Co., Ltd., baked scallop powder] T: Diatomaceous earth (manufactured by Nippon Diatomaceous Earth Construction Materials Co., Ltd., product name: Eco Queen)

[0090] The building material composition obtained above was filled into a mold measuring 8 cm in length, 16 cm in width and 5 mm in depth, and a mold heated to 100°C was placed on top of the filled material. The molded building material was hot pressed until no more water vapor was released, producing a building material measuring 16 cm in length, 8 cm in width and 5 mm in thickness.

[0091] The physical properties of the building material obtained above were examined in terms of impact resistance, bending resistance and brittleness according to the following methods. The results are shown in Table 1.

[0092] [Impact resistance] The bottom surface of the building material obtained above, 1 cm from the short sides of both ends, was placed on a rectangular iron stand, and a steel ball (mass: 200 g) was dropped from a position 1 m above the top surface of the building material toward the center of the building material. The top surface of the building material that had come into contact with the steel ball was visually observed, and the impact resistance was evaluated based on the following evaluation criteria. (Evaluation Criteria) ◎: No abnormalities on the surface of the building material. ◯: There are slight dents on the surface of the building material, but no cracks are observed in the building material. △: Clear dents are observed on the surface of the building material, but no cracks are observed in the building material. ×: Cracks were observed in the building materials.

[0093] [Bending resistance] A section 1 cm from the short side of one end of the building material obtained above was fixed in a vice, a clamp was attached to the short side of the other end of the building material, a hanging scale (manufactured by Dr. Meter, product number: ES-PS01) was attached to the clamp, and the hanging scale was pulled in a direction perpendicular to the plane of the building material. The stress (measured value on the scale) when the building material bent was measured, and the bending resistance was evaluated based on the following evaluation criteria. (Evaluation Criteria) ◎: The stress (measured on a scale) when the building material bends is 4 kg or more. ○: The stress (measured on a scale) when the building material bends is 3kg or more and less than 4kg. △: The stress (measured on a scale) when the building material bends is 2.5 kg or more and less than 3 kg. ×: The stress (measured on a scale) when the building material bends is less than 2.5 kg.

[0094] [Brittleness] When attaching a tapping screw (made of stainless steel, nominal diameter D: 5 mm, nominal length L: 16 mm) to the building material obtained above with an electric screwdriver (manufactured by Powerland, product number: D018SS), the speed scale of the electric screwdriver was changed, and the speed scale was read when the screw began to spin freely, and the brittleness was evaluated based on the following evaluation criteria. (Evaluation Criteria) ◎: The screw does not spin freely even when the electric screwdriver's gear shift scale (clutch) is set to 3 or higher. ○: When the electric screwdriver's gear shift scale (clutch) is set to 3, the screw spins freely. △: When the electric screwdriver's gear shift scale (clutch) is set to 2, the screw spins freely. ×: When the electric screwdriver's gear shift scale (clutch) is set to 1, the screw spins freely.

[0095] [Table 1]

[0096] The results shown in Table 1 show that when the binders for building materials obtained in each Example were used, building materials having high impact resistance, excellent bending resistance, and low brittleness were obtained.

Claims

1. The binder for building materials is characterized in that it contains an aqueous polyvinyl alcohol solution having a polyvinyl alcohol concentration of 5 to 20 mass % and a polyvinyl alcohol-based resin powder, the content of the polyvinyl alcohol-based resin powder in the binder for building materials is 10 to 45 mass %, and a cross-linked polyvinyl alcohol powder is used as the polyvinyl alcohol-based resin powder.

2. The two-component binder for use in building materials is characterized in that it comprises a component A containing an aqueous polyvinyl alcohol solution having a polyvinyl alcohol concentration of 5 to 20% by mass, and a component B containing a polyvinyl alcohol-based resin powder, the amount of the polyvinyl alcohol-based resin powder being 10 to 85 parts by mass per 100 parts by mass of the aqueous polyvinyl alcohol solution, and a cross-linked polyvinyl alcohol powder is used as the polyvinyl alcohol-based resin powder.

3. A composition for building materials, comprising the binder for building materials according to claim 1 or 2 and a filler.

4. A building material formed from the building material composition according to claim 3.

Citation Information

Patent Citations

  • Aqueous dispersion of polyvinyl alcohol and production thereof

    JP1981167745A

  • Binder

    JP2003238921A

  • Method for manufacturing building material using recyclable material and building material

    JP2013227188A

  • Gypsum board

    WO2011052048A1