How to make carbon fiber from paper products
A method for producing carbon fibers from recycled paper using direct dissolution in phosphoric acid and solvent spinning addresses the cost and environmental inefficiencies of traditional methods, achieving high mechanical properties at reduced costs.
Patent Information
- Application Number
- JP2021566233
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-05-10
- Filing Date
- 2020-05-07
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2040-05-07
AI Technical Summary
Existing methods for producing carbon fibers from cellulose are costly and environmentally inefficient, lacking a sustainable and cost-effective process that maintains adequate mechanical properties.
A method is developed to produce carbon fibers from recycled paper products by directly dissolving crushed paper in an aqueous phosphoric acid solution, followed by solvent spinning and carbonization, eliminating pre-treatment steps and reducing the need for high temperature processes.
This method produces carbon fibers with mechanical properties exceeding 1,200 MPa tensile strength and 75 GPa Young's modulus, suitable for composite materials, at a significantly lower cost and environmental impact compared to traditional methods.
Abstract
Description
[Technical field]
[0001] The present invention is in the general field of carbon fiber manufacturing and is specifically directed to the preparation of composite materials from bio-based materials.
[0002] More particularly, the present invention relates to a method for producing carbon fibers from paper products, and more generally to a method for producing composite articles based on carbon fibers dispersed in an organic polymer resin matrix, which method comprises carrying out the method for producing carbon fibers according to the present invention. [Background technology]
[0003] Carbon fibres are used in many areas to exploit their particularly favourable mechanical, electrical and thermal properties, as well as their low weight.
[0004] To avoid the predicted problem of depletion of fossil resources, the production of carbon fibres from renewable bio-based materials has been the subject of much research in the last decades. In particular, the prior art has proposed the production of such fibres from cellulose, the polymeric carbohydrate that makes up the cell walls of plants and the main component of wood. Cellulose is the most abundant organic material on earth. Carbon fibres obtained from cellulose have the particular advantage of being very well structurable. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] International Publication No. 2018 / 142025 [Patent Document 2] International Publication No. 2014 / 162062 [Patent Document 3] U.S. Pat. No. 5,601,767 [Patent Document 4] International Publication No. 85 / 05115 [Patent Document 5] U.S. Patent No. 5,817,801 [Patent Document 6] U.S. Patent No. 5,804,120 [Non-patent literature]
[0006] [Non-Patent Document 1] Boerstel, Polymer, 42:7371-7379, 2001 [Non-Patent Document 2] Swatloski, JACS, 124:4974-4975, 2002 Summary of the Invention [Problem to be solved by the invention]
[0007] The present invention aims to provide a method for producing continuous carbon fibres from cellulose at low cost and in the most environmentally friendly manner possible, with sufficiently good mechanical properties, which fibres are used in many applications, in particular for producing articles made of composite materials. [Means for solving the problem]
[0008] To this end, the inventors are investigating the paper recycling industry.
[0009] More specifically, paper is composed of about 70-85% cellulose fibers extracted from wood or recycled paper. The remaining 15-30% are mineral filler-type additives, mainly consisting of carbonates, as well as various additives such as adhesives, starches, pigments, etc., that are added during the manufacture of the paper to give it certain properties.
[0010] Currently, a very large amount of paper is consumed worldwide to produce paper products, especially printing paper, packaging paper, sanitary paper and household paper, as well as sanitary and medical products. Therefore, recycling paper products, especially waste paper products, is ecologically and economically important, especially from the perspective of carbon fiber production. Indeed, the cost price of waste paper is much lower than that of traditional precursor materials, such as refined cellulose or polyacrylonitrile, used to produce carbon fibers, especially in the paper industry.
[0011] WO 2018 / 142025 describes a method for preparing cellulose fibers from everyday cellulose waste that can be used as a precursor for carbon fibers. The method includes an initial step of treating the waste by digestion in an alkaline glycerol solution, followed by dissolving the resulting cellulose pulp in an ionic liquid, and spinning the resulting solution to form cellulose fibers.
[0012] WO 2014 / 162062 describes a method for producing cellulose fibers from lignocellulosic materials, which involves dissolving the materials in a specific solvent, a diazabicyclononene-based ionic liquid, and spinning the resulting solution to form cellulose fibers.
[0013] US Patent No. 5,601,767 describes a method for making cellulose fibers from paper, which involves dissolving shredded paper in an aqueous amine oxide solution, removing the water by drying at high temperature, and forming cellulose fibers by solvent spinning. However, this document does not mention that the cellulose fibers can be used to form carbon fibers.
[0014] The inventors have discovered that it is possible to recover the cellulose contained in the manufactured paper products in a sufficiently nearly undecomposed form to form individual and continuous cellulosic fibers, so that they can be used in conventional spinning processes, as is usually the case with paper cellulose pulp, and then to subject the cellulosic fibers to carbonization in order to obtain carbon fibers with fairly satisfactory mechanical properties and with a good carbon yield during the carbonization step. More specifically, the inventors have discovered that, contrary to what is recommended in the prior art for producing cellulose fiber precursors for carbon fibers, such results can be obtained under certain operating conditions, with a minimum number of steps, without carrying out pretreatment steps, such as, in particular, digestion, washing, pulping of the manufactured products or the cellulose contained therein, before the spinning step, and without requiring significant temperature inputs other than the carbonization step itself. In particular, these carbon fibers can be used to produce composite materials. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Therefore, the present invention proposes a method for producing carbon fibers by recycling paper products.
[0016] As used herein, the term "paper product" is understood to mean any manufactured product made from paper pulp, such as, but not limited to, office or printing paper products, including printed matter and envelopes, paper towels, paper tissues, toilet paper, paper napkins, and the like.
[0017] The term "paper product" does not include pulp obtained directly from wood by chemical or mechanical processes practiced in the paper industry.
[0018] The manufactured products used in the method according to the invention may be new products or used products, in particular those at the end of their life.
[0019] The method for producing carbon fiber according to the present invention comprises the steps of: a) preparing a cellulosic fiber comprising the steps of: a1) crushing / shredding the paper product to obtain crushed paper material; a3) directly dissolving the ground material obtained at the end of step a1) in an aqueous solution of phosphoric acid, which acts as a solvent solution for dissolving the cellulose, to form a so-called spinning solution; a4) using the spinning solution to carry out a solvent spinning process, also commonly referred to as a wet spinning process, to produce continuous cellulose fibers; and a5) optionally drawing the resulting continuous cellulosic fibers to form longer fibers, the implementation of such a drawing step being a particularly preferred step within the scope of the present invention; preparing a cellulosic fiber comprising: b) carbonizing the resulting continuous cellulosic fibers to form carbon fibers; Includes.
[0020] The expression "dissolving the ground material directly in an aqueous phosphoric acid solution" is understood in this specification to mean that the ground material obtained at the end of step a1) is dissolved directly in the aqueous solution without being subjected to one or more prior treatment steps.
[0021] The solvent spinning process, i.e. the wet spinning process, carried out in step a4) of the method according to the invention, consists in extruding the spinning dope in a manner conventional per se through a spinneret into a so-called coagulation bath, which contains a non-solvent for cellulose which is miscible with the solvent solution used to prepare the spinning dope, i.e. the aqueous phosphoric acid solution.
[0022] The solvent spinning process carried out according to the invention may be a so-called "wet" process, in which the spinneret is immersed in the coagulation bath, or a so-called "dry jet" process, in which the spinneret is typically positioned at a distance of 1 mm to 20 cm above the coagulation bath.
[0023] The method for producing carbon fibers according to the invention is simple to carry out and each step can be carried out by techniques known to those skilled in the art. Carbon fibers having excellent properties, especially mechanical properties, can be formed in a very small number of steps and at particularly advantageous costs, which are much less than those required to produce carbon fibers using conventional precursor materials from the paper industry, such as purified cellulose or polyacrylonitrile.
[0024] In particular, the method according to the invention comprises the step of preparing continuous cellulose-based fibers, inducing a molecular rearrangement in the fibers, resulting in a crystalline structure of cellulose in the fibers, resulting in a final carbon fiber with very good mechanical properties. In particular, the method according to the invention results in carbon fibers with a tensile strength of more than 1,200 MPa, a Young's modulus of more than 75 GPa, and even a tensile strength of more than 2,500 MPa and a Young's modulus of more than 200 GPa after graphitization. These mechanical properties are suitable for use in fields of application where high strength materials are required. None of the prior art has proposed that such sufficient mechanical properties can be obtained with such a small number of steps, namely, the steps of crushing the manufactured paper product, dissolving the crushed material in an aqueous phosphoric acid solution without any other pretreatment, and solvent spinning the resulting solution.
[0025] More generally, the carbon fibres obtained by the production process according to the invention can be used in many sectors, in particular to produce materials or parts intended for use in sectors as diverse as construction and infrastructure, industrial equipment, automotive, rail or shipping transport, electrical and electronics, sports and leisure, renewable energies, in particular wind power, etc. For this purpose, they can be used as they are, or can be assembled in non-woven or woven or knitted form, and can be mixed with other types of fibres if necessary.
[0026] Due to their low cost, the carbon fibres obtained by the process according to the invention can be advantageously used to replace glass fibres in applications where it is necessary to use reinforcing fibres with moderate tensile strength and low production costs. For example, the carbon fibres obtained by the process according to the invention can be used to manufacture structures in the field of construction or renewable energy production, such as wind or marine turbine blades, replacing all or part of the glass fibres used up to now. The carbon fibres according to the invention can be used, for example, to replace 5 to 40%, in particular 10 to 30%, of these glass fibres.
[0027] The invention therefore particularly relates to wind turbine blades or marine turbine blades of large dimensions, i.e. at least 30 meters long, typically 40 to 100 meters long. These turbines are made from a composite material made of reinforcing fibres dispersed in a polymer resin matrix, containing, as reinforcing fibres for the blades, 5 to 40%, preferably 10 to 30%, of cellulose-based carbon fibres obtained by the process according to the invention, the remainder of the reinforcing fibres being constituted by glass fibres. The latter are typically made up of two half-blades. The density of these cellulose-based carbon fibres is between 1.3 and 1.8 g / m 3 It is preferred and advantageous that the density of the glass fibre is about 2.2 g / m 3 It is understood that the above percentage of cellulose-derived carbon fibers obtained according to the invention relative to the total amount of reinforcing fibers is defined for the reinforcing fibers of the blade airfoil and is in addition to the percentage of carbon fibers contained in the resin-carbon composite spar (commonly called "spar cap"), which is incorporated inside the blade for large blades, in the volume defined by the half blades.
[0028] The proportion and distribution of cellulose-derived carbon fibers in the blade is calculated according to several criteria, in particular the dimensional and mechanical properties, the weight of the wind turbine, the size, the energy of the motor and the target power (advantageously 3-8 MW).
[0029] The resulting blade for a wind turbine or similar structure (eg, a marine turbine) has a targeted length and mechanical properties that reduce the power requirements of the motor of the structure.
[0030] The method according to the invention can further comprise one or more of the following features, taken alone or in any technically possible combination:
[0031] The crushing / shredding of the paper products carried out in step a1) of the process according to the invention can be carried out according to any method known to the person skilled in the art, for example by means of mills / shredders which are conventional per se.
[0032] Preferably, in step a1), the crushing is carried out in such a way as to obtain a crushed material formed from particles, the largest dimension of which is between 100 and 1,000 μm, preferably between 200 and 500 μm. These particles are preferably non-agglomerated.
[0033] This step can be preceded by various operations to clean and / or dedust the paper product, as well as by cutting operations.
[0034] The crushed material thus obtained is dissolved directly in the spinning solution.
[0035] The method according to the invention is therefore particularly advantageous compared to the methods proposed in the prior art for preparing cellulose, which include extensive purification steps, for the purpose of producing carbon fibers from lignocellulosic biomass. The time and costs required to produce carbon fibers with the method according to the invention are therefore much less than the traditional methods for preparing carbon fibers from lignocellulosic biomass. In particular, the cost of the cellulose raw material subjected to the spinning process is significantly less than the traditional methods for preparing carbon fibers.
[0036] Alternatively, the method for producing carbon fibres may, although this is not essential, comprise, after step a1) of crushing the paper product and before step a3) of preparing the spinning solution, a step a2) of pre-treating the crushed material obtained, in order to reduce its mineral filler content, preferably to a value of less than or equal to 1%, preferentially to a value of less than or equal to 0.3%. The mineral filler content of the crushed material can be determined in a manner conventional per se for the person skilled in the art, for example by thermogravimetric analysis at 500° C. to 1,000° C. in air, before, during or after the pre-treatment step.
[0037] The step a2) of pre-treating the shredded material can be carried out by any conventional process for refining paper, retaining substantially only cellulose.
[0038] The step a2) of pre-treating the shredded material may comprise pulping this material to obtain a paper pulp, followed successively by hyperwashing, drying and crushing, each of which may be carried out by any method known to those skilled in the art.
[0039] The pulping of the shredded paper material can be carried out, for example, by a pulper, for example of the type equipped with cross blades, drum pulper type or spiral pulper type, in which the shredded material suspended in the aqueous solution is stirred, for example for about 15 minutes. The shredded material can be left pre-soaked in the aqueous solution, for example for 15 minutes to 4 hours. The aqueous solution can optionally contain one or more additives, such as sodium hydroxide, hydrogen peroxide, silicates, fatty acids and / or any other deinking additives.
[0040] In the process of pulping the shredded paper material, the paper is mechanically broken down and the contained cellulose fibers are placed in aqueous suspension, preferably under conditions to obtain a pulp containing about 2% by weight of paper.
[0041] Globally, the hyper-washing process consists of cleaning the paper pulp with large amounts of water, retaining only the contained cellulose fibers and removing the mineral fillers and other contaminants.
[0042] Hyper-washing can be performed, for example, using a diffuser, where the pulp is placed on a screen and then washed with a large amount of water until the wash water is clean. Alternatively, hyper-washing can be performed by a centrifugal dewatering machine, a rotating drum with a cloth bag containing the paper pulp placed inside. Water is injected into the rotating drum. Such an implementation has the particular advantage of hyper-washing a large amount of pulp and dewatering the pulp once it is clean, resulting in a pulp that contains a small amount of water.
[0043] Any other conventional hyper-cleaning method may be performed in other ways.
[0044] Optionally, the hyperwash step can be followed by a step of concentrating the cellulose pulp, for example by centrifugation or filtration; and / or a step known as swelling the pulp, which consists of mechanically opening its structure.
[0045] Drying of the resulting pulp can be carried out, for example, in an oven, preferably until the moisture content of the pulp is less than 20%, preferably less than 10%. When the initial moisture content of the pulp is very high, the oven drying can be preceded by pulp dewatering, in particular in a rotary drum, to reduce the moisture content to a value of about 60% or less.
[0046] Moisture content is defined herein in the conventional manner as the percentage by weight of water contained in the pulp, based on the total weight of the pulp, at a relative humidity of 60% air and at about 20° C. In particular, this moisture content can be determined by comparing the weight of a pulp sample with the weight of the same sample after a drying step above 100° C. until a substantially constant sample weight is obtained.
[0047] After drying, the paper pulp can be mechanically crushed / shredded to form a crushed material and step a3) of the method according to the invention is carried out to form the spinning solution.
[0048] In the configuration where the product is formed from an inked paper, the method for producing carbon fibers can include a flotation step of the paper pulp after the pulping step to remove the contained ink, which can be carried out by any method known to the person skilled in the art.
[0049] If the method according to the invention does not include a step a2) of pretreating such shredded paper material, the solvent spinning process is advantageously easier to carry out and the carbon fiber production yield is equally high compared to a method including such a pretreatment step, so the method according to the invention advantageously combines speed, efficiency and low cost.
[0050] Preferably, the crushed material dissolved in the solvent solution in step a3) of the process according to the invention contains more than 90% by weight, preferably more than 95% by weight, of cellulose, based on the total weight of the crushed material. Its water content is preferably less than or equal to 15% by weight, based on the total weight of the crushed material. Its mineral content is preferably less than or equal to 0.3% by weight, preferentially less than or equal to 0.1% by weight, based on the total weight of the crushed material. Such features are favorable for improving the mechanical properties of the carbon fibers obtained by the process according to the invention.
[0051] The paper products used in the method according to the invention may be formed from recycled paper.
[0052] Alternatively, it may be made from paper resulting from chemical paper pulp, especially kraft or bisulfite pulp, for example writing or printing paper. Chemical paper pulp is obtained by cooking wood with chemicals. There are two main processes: the acid process, which produces bisulfite pulp, and the kraft process, which involves cooking wood in a liquor containing sodium hydroxide and sodium sulfide.
[0053] Step a3) of dissolving the ground material obtained at the end of step a1) of the process uses an aqueous phosphoric acid solution as a solvent solution for the cellulose.
[0054] Other conventional solvent solutions are zinc chloride solution, formic acid, N-methylmorpholine-N-oxide (NMMO), ionic liquids, or any mixture thereof technically possible.
[0055] As a solvent solution, the aqueous phosphoric acid solution preferably has a phosphoric acid concentration of 75-99% by volume, based on the total volume of the aqueous solution, which surprisingly enough alone is sufficient to obtain carbon fibers having particularly advantageous mechanical properties from the manufactured paper product, which has been subjected to a simple crushing step before being dissolved in the solvent solution.
[0056] Dissolution of the ground material in the solvent solution can be facilitated by heat treatment, for example by heating under vacuum by conventional methods followed by cooling to very low temperatures.
[0057] However, this heat treatment is preferably limited to temperatures below 45°C.
[0058] More generally, in step a) of preparing the cellulosic fibres, the temperature applied to the cellulose does not exceed 45° C. This gives particularly good mechanical properties of the final carbon fibres, together with the advantage of low energy consumption.
[0059] In a specific implementation of the invention, the spinning solution is subjected to a solvent spinning process without a prior drying step specifically intended to remove water, thus advantageously minimizing the number of steps in the method according to the invention.
[0060] The spinning solution is preferably not subjected to any further processing prior to the spinning itself, except for mixing additional elements into the solution as described below. Optionally, filtration can also be performed. In a preferred embodiment of the present invention, the spinning solution is not filtered prior to spinning.
[0061] In a preferred embodiment of the invention, the shredded material is mixed with purified cellulose in step a3) by dissolving the shredded material in a solvent solution consisting of an aqueous solution of phosphoric acid.
[0062] The term purified cellulose is understood in this specification to mean cellulose obtained from lignocellulosic biomass, in particular so-called paper cellulose, i.e. cellulose obtained from the papermaking process and having a higher purity than the cellulose contained in the crushed material obtained according to the invention, which is commonly used in prior art methods for producing carbon fibers.
[0063] The refined cellulose used in connection with the present invention can be obtained from annual hard or softwood plants, such as straw or cotton, and can be obtained by any conventional method, such as the Kraft or sodium hydroxide cooking methods.
[0064] In the mixture of ground material and purified cellulose that is mixed with the spinning solution, the purified cellulose is preferably present in an amount of from 20 to 90% by weight, preferably from 40 to 60% by weight, for example about 50% by weight, based on the total weight of the mixture of ground material and purified cellulose.
[0065] The total amount of ground material dissolved in the solvent in step a3) of the process, or, where appropriate, the total amount of the mixture of ground material and purified cellulose added, is from 1 to 50% by weight, preferably from 5 to 30% by weight, preferentially from 5 to 20% by weight, for example from 5 to 15% by weight, based on the total weight of the resulting spinning solution.
[0066] The concentration of the ground material or, where appropriate, the mixture of ground material and purified cellulose dissolved in the solvent medium in step a3) of the process according to the invention is therefore from 1 to 50% by weight, preferably from 5 to 30% by weight, preferentially from 5 to 20% by weight, for example from 5 to 15% by weight, based on the total weight of the resulting spinning solution.
[0067] The shredded paper or paper pulp material can also be mixed with substances other than refined cellulose, such as polyacrylonitrile, to advantageously obtain carbon fibers with further improved mechanical properties, in particular tensile strengths after graphitization of more than 4,000 MPa, which are particularly suitable for use in applications requiring very high material strength, such as for producing hydrogen tanks.
[0068] The method according to the invention may involve the addition of one or more additives to the spinning solution to provide better structuring of the material, improved mechanical properties of the fibers formed, etc.
[0069] Each of these additives may be present in the spinning solution in particular in a content of from 1 ppm to 10% by weight, based on the total weight of the spinning solution, preferably from 1 ppm to 5% by weight, for example from 100 ppm to 1% by weight, based on the total weight of the spinning solution.
[0070] Examples of additives that can be added to the spinning solution according to the invention include compatibilizers such as maleic anhydride grafted polymers or copolymers, in particular Lotader® 3300, commercially available from Arkema, or Beiwa® 901 from DzBh.
[0071] In a specific embodiment of the invention, the spinning solution contains a non-ionic emulsifier, preferably at a concentration of 0.1 to 1% by weight, for example about 0.2% by weight, based on the weight of the ground material dissolved in the solvent solution in step a3), and if appropriate based on the weight of the mixture of ground material and purified cellulose. The spinning solution may contain one or more emulsifiers, for example those sold under the trade name Emran® by BASF.
[0072] Before carrying out the next step of the method according to the invention, the spinning solution may be filtered to remove solid particles.
[0073] In a specific implementation of the invention, one or more nanosized carbonaceous fillers are added to the spinning solution during step a3) of the method according to the invention or immediately before or after it. The nanosized carbonaceous fillers are added to the spinning solution in an amount of preferably 1 ppm to 30% by weight, based on the weight of the ground material dissolved in the solvent solution in step a3) and, where appropriate, based on the weight of the mixture of ground material and purified cellulose. This concentration is preferentially 0.001 to 5% by weight, in particular 0.01 to 5% by weight.
[0074] The expression "nanosized carbonaceous filler" is understood in this document to mean a filler comprising one of the members of the group consisting of single- or multi-walled carbon nanotubes, carbon nanofibers, graphene, graphene oxide, reduced graphene oxide, fullerenes, cellulose nanofibrils, cellulose nanocrystals and carbon black, or any mixture of these elements. Preferably, the nanosized carbonaceous filler mixed into the spinning solution according to the invention is carbon nanotubes, alone or in a mixture with graphene. Carbon nanotubes are commercially available, for example from Arkema under the trade name Graphistrength®.
[0075] The nanosized carbonaceous fillers according to the invention may have a smaller dimension of 0.1 to 200 nm, preferably 0.1 to 160 nm, preferentially 0.1 to 50 nm, which dimension can be measured, for example, by light scattering methods.
[0076] The term "graphene" is understood according to the invention to mean discrete graphite sheets separated in a plane, but also aggregates containing one to several tens of sheets by extension and having a planar or approximately corrugated structure. This definition therefore includes FLGs (few-layer graphene), NGPs (nanographene plates), CNSs (carbon nanosheets) and GNRs (graphene nanoribbons). However, it excludes carbon nanotubes and nanofibers, respectively, which are constituted by the concentric winding of one or more graphene sheets and the turbostratic stacking of these sheets.
[0077] It is preferred that the nanosized carbonaceous filler be incorporated into the spinning dope of the present invention in the form of a water or solvent based liquid dispersion.
[0078] Dispersion of the nano-sized carbonaceous fillers can be carried out by ultrasonic probe, ball mill, high shear mixer, or any other conventionally used equipment, optionally in the presence of a surfactant.
[0079] The spinning process carried out in step a4) of the method according to the invention to form continuous cellulose fibres may be of any type known to the person skilled in the art.
[0080] As mentioned above, in this process, the spinning solution is injected statically or flow-through through a spinneret consisting of one or more holes into a coagulation bath either directly (wet spinning) or through an air gap (dry jet wet spinning). Upon contact with the coagulation bath, the fibers coagulate. This is advantageous for producing continuous cellulosic fibers.
[0081] The coagulation bath employed can have any conventional composition that is compatible with the phosphoric acid in the spinning solution to effect the particular type of solvent spinning process.
[0082] For example, the coagulation bath can be made of isopropanol, water, acetone, or any other solvent that will coagulate cellulose upon contact, or any mixture thereof.
[0083] Other conventional solvent spinning processes include the viscose process, the lyocell process, or processes that use ionic liquids as the solvent for the spinning solution.
[0084] Specific examples of conventional solvent spinning processes are described in particular in WO 85 / 05115, US Pat. No. 5,817,801, US Pat. No. 5,804,120, or in publications by Boerstel, 2001 in Polymer, 42:7371-7379, or Swatloski, 2002 in JACS, 124:4974-4975.
[0085] In a specific embodiment of the invention, the spinning dope is formed from phosphoric acid, optionally in the presence of a non-ionic emulsifier, and the coagulation bath is formed from isopropanol alone or in admixture with water.
[0086] The continuous cellulosic fibers obtained by the spinning process according to the invention can be in the form of monofilaments or multifilaments and can then be washed and dried.
[0087] Optionally, a drawing step a5) is carried out to form longer fibres.
[0088] The fiber drawing process can be carried out according to any method and by any equipment for carrying out such operations known to the person skilled in the art. In particular, it can be carried out at a temperature at which the material constituting the fiber is softened. For this purpose, the fiber passes through an oven heated to said temperature, passes through a table of so-called feed rollers and then successively through a table of so-called stretching rollers. Depending on the rotation speed ratio of the feed rollers and the stretching rollers, it undergoes drawing between the two tables of rollers. Alternatively, it can be drawn on heated rollers rotating at different speeds.
[0089] Such stretching favors alignment of the polymer chains along the fiber axis.
[0090] The fibers can optionally be treated with radiation, such as gamma, beta, electron beam, or ultraviolet light, at the end of the spinning process.
[0091] The resulting cellulosic fibers are quite long and can then be wound, for example, onto a cardboard tube.
[0092] The cellulosic fibers obtained according to the present invention can then be sized in a conventional manner prior to the carbonization step to obtain continuous carbon fibers.
[0093] According to an alternative embodiment of the present invention, the nano-sized carbonaceous fillers are introduced into the sizing bath and not into the spinning solution as described above.
[0094] Step b) of carbonizing the continuous cellulosic fibers of the process according to the invention is carried out in a conventional manner, using any combination of operating parameters for carbonizing cellulose fibers described in the prior art.
[0095] It is preferably carried out in an inert atmosphere.
[0096] Carbonization can be carried out continuously, with the fibers passing through a carbonization furnace, or discontinuously, i.e. statically, with the fibers preferably under tension in the furnace.
[0097] Before carbonization, the continuous cellulosic fibers can be impregnated with one or more additives, in particular with so-called carbonizing agents. The impregnating agents serve to increase the mechanical properties of the final carbon fibers and to increase the carbon yield of the carbonization process. These additives are conventional per se. By way of example, the cellulosic fibers can be impregnated with one or more of the following additives: Brönsted acid compounds or compounds which release Brönsted acids on heating, in particular hydrogen halides, halides with any counterion such as sodium, potassium or ammonium, sulfuric acid, sulfates with any counterion such as sodium, potassium or ammonium, organic sulfonic acids with alkyl groups such as methylsulfonic acid or organic sulfonic acids with aryl groups such as paratoluenesulfonic acid or organic sulfonic acids with any other organic groups, organic sulfonates corresponding to the abovementioned sulfonic acids and with any counterion such as sodium, potassium or ammonium, phosphoric acid and polyphosphoric acid and / or phosphates and polyphosphates with any counterion such as sodium, potassium or ammonium; Lewis acid compounds, in particular boric acid and / or aluminum chloride AlCl 3 or ferric chloride FeCl 2 The formulations may be impregnated with metal halides such as metal halides, urea, nano-sized carbonaceous fillers, and / or siliconized polymer bases, such as polydimethylsiloxane bases, especially in combination with crosslinkers. Such a list is in no way limiting.
[0098] Impregnation additives based on siliconized polymers are particularly preferred in the context of the present invention, since they are able to further improve the mechanical properties of the carbon fibers obtained according to the invention.Preference is given to using impregnation additives of the siliconized type in a proportion, defined as the weight percentage of the additive based on the total weight of the cellulose fibers and the additive, of 0.01 to 20% by weight, preferably 0.5 to 10% by weight, more preferably 1 to 5% by weight.
[0099] Carbonization can be carried out at a temperature of 1,000 to 1,500° C., with or without a stabilization step prior to carbonization in air at a temperature of about 250° C.
[0100] In a specific embodiment of the present invention, the carbonization furnace is sealed and heated under vacuum at 1.10 4 The pressure in the furnace is then adjusted to less than 0.1 bar. The furnace is then filled with an inert gas such as nitrogen or argon, and the gas is leaked out so that the gas flow rate is 50 to 500 changes in the furnace volume per hour. The pressure in the furnace is preferably 1.10 3 Pa to 5.10 4 The pressure is preferably above 800 Pa. The temperature applied in the carbonization furnace is preferably between 800° C. and 1,500° C.
[0101] This carbonization process produces carbon fibers.
[0102] The carbon fibres can then optionally be subjected to a graphitisation treatment in order to obtain a better structuring of the carbon and therefore more favourable mechanical properties, which can be carried out, for example, by heating the fibres in an inert gas to a temperature of 2,000 to 3,000° C., for example for a period of 30 seconds to 10 minutes.
[0103] Otherwise, the cellulosic fibers according to the invention can be continuously carbonized by passing them successively through various furnaces, including a carbonization furnace at temperatures between 800° C. and 1,500° C., followed by a graphitization furnace at temperatures up to 2,500° C., under an inert atmosphere. The speed at which the fibers pass through these furnaces is therefore preferentially between 0.1 and 10 m / h.
[0104] The carbon fibres obtained using the method according to the invention can have a diameter of 5 to 30 μm and a length of several metres.
[0105] In a particular embodiment of the invention, the method comprises forming a web of cellulosic fibers from the plurality of continuous cellulosic fibers obtained in step a4) or a5), after which step b) of carbonizing the continuous cellulosic fibers is carried out by carbonizing the web of continuous cellulosic fibers to form a carbon fiber-based web.
[0106] Webs formed from cellulosic fibers according to the present invention can be of any shape and size. The fibers can be arranged in woven fabrics, such as taffeta, twill, satin, etc., with different weights and weaves used alone or in combination, or in nonwoven fabrics, felts or films, for example, where the fibers are all oriented in the same direction, or where the fibers are randomly oriented. These are known as unidirectional webs.
[0107] The continuous cellulosic fibers according to the present invention can be used in the web alone or in combination with other types of fibers.
[0108] Carbonization of the web of continuous cellulosic fibers can be carried out by any carbonization process known to those skilled in the art, either statically or by continuous movement through a carbonization furnace. For carbonization of webs of continuous cellulosic fibers according to the present invention, the features described above with respect to the treatment of individual fibers apply in an analogous manner.
[0109] The webs of continuous cellulosic fibers according to the present invention can be carbonized individually or can be carbonized as flat stacked webs, or as stacked webs after being formed into a desired shape if desired.
[0110] Another aspect of the invention relates to carbon fibres obtainable by the process according to the invention and having one or more of the above mentioned characteristics.
[0111] The carbon fibres are interconnected and can have a diameter of 1 to 1,000 μm, preferably 15 to 30 μm, and a length of several metres.
[0112] It may advantageously have a tensile strength of more than 1,200 MPa, preferably 2,000 MPa or more after graphitization, and / or a Young's modulus of more than 75 GPa, preferably 200 GPa or more after graphitization, these parameters being measured according to method B of the international standard ISO 11566.
[0113] Another aspect of the invention relates to continuous cellulosic fibers obtained at the end of process step a) as intermediate product during the implementation of the process for producing carbon fibers according to the invention, said cellulosic fibers being made from recycled paper products, alone or mixed with other constituents such as those listed above.
[0114] The continuous cellulosic fibres may have a diameter of between 10 and 30 μm and / or a strength of between 10 and 40 cN / tex and / or a Young's modulus of between 10 and 30 GPa, these parameters being measured in accordance with the international standard ISO 2062.
[0115] It can be conveniently stored and transported.
[0116] According to another aspect, the invention relates to a carbon fiber web obtained from the carbon fibers according to the invention, the carbon fibers being woven or knitted together or juxtaposed in a nonwoven fabric.
[0117] Another aspect of the present invention relates to a carbon fiber web obtainable by the method for producing carbon fibers according to the present invention, comprising the steps of forming a web of cellulosic fibers from a plurality of continuous cellulosic fibers obtained in step a4) or a5) of the method, and carbonizing the web of continuous cellulosic fibers to form a carbon fiber based web.
[0118] Furthermore, the invention relates to three-dimensional fiber structures obtained by stacking a plurality of webs of continuous cellulosic fibers according to the invention or by stacking a plurality of carbon fiber webs according to the invention, which can be shaped as required to form a preform, for example for the manufacture of an article made of a composite material containing reinforcing fibers dispersed in a binder.
[0119] According to another aspect, the present invention relates to the use of the carbon fibers or carbon fiber webs according to the invention to manufacture articles made of composite materials containing carbon fibers dispersed in an organic polymer resin matrix.
[0120] Yet another aspect of the invention relates to a method for producing a composite article containing carbon fibers dispersed in an organic polymer resin matrix, comprising carrying out a method for producing carbon fibers according to the invention, comprising producing carbon fibers by carbonization of individual continuous cellulosic fibers, and forming a carbon fiber web from a plurality of the carbon fibers thus obtained; or carrying out a method for producing carbon fibers according to the invention, comprising forming a web of continuous cellulosic fibers and carbonizing the web of fibers to form a carbon fiber web; and producing a composite article from a plurality of the carbon fiber webs thus obtained.
[0121] The manufacture of composite articles from the carbon fiber webs obtained according to the invention can be carried out by any method conventional to those skilled in the art.
[0122] A composite material is defined herein in the conventional way, i.e. as an assembly of several different materials or basic components bonded together, more specifically consisting of long, mechanically strong fibers, in this case carbon fibers, dispersed in an organic polymer resin matrix. The term resin is used herein to define a polymeric compound, which may be of the thermoplastic or thermosetting type, acting as a structural adhesive in which the fibers are dispersed in a more or less organized manner. The composite material thus formed has its own mechanical properties and is very advantageous in terms of mechanical strength and lightness.
[0123] Generally, the manufacture of such composite materials consists of forming a stack of several webs of carbon fibers impregnated with an unpolymerized organic resin into the desired shape under conditions, particularly temperature conditions, which cause the resin to polymerize.
[0124] The composite article according to the invention can be produced in a conventional manner, for example by using the technique of draping layers pre-impregnated with resin, followed by polymerization of the assembly in an autoclave to form a composite, at least some of these layers being composed of the carbon fiber web according to the invention, or it can be produced by resin infusion or impregnation techniques, in particular resin transfer molding (RTM) techniques, with dry fiber layers, some of these layers being composed of the carbon fiber web according to the invention.
[0125] The composite materials produced according to the invention may be of monolithic type and / or of sandwich type, for example having a honeycomb structure.
[0126] The fibers may be arranged in the present invention into woven fabrics having different weights and weaves, used alone or in combination, such as taffeta, twill, satin, etc., or nonwoven fabrics, for example, where the fibers are all oriented in the same direction.
[0127] The carbon fibers obtained according to the present invention may be implemented alone or in combination with one or more other types of fibers, and any configuration of such combinations is within the scope of the present invention.
[0128] Any conventional resin can be used in the context of the present invention, in particular a thermosetting resin, such as an epoxy resin, a phenolic resin or a mixture thereof, or a thermoplastic resin.
[0129] According to another aspect, the invention relates to an article made of a composite material containing carbon fibers dispersed in an organic polymer resin matrix obtained by the manufacturing process according to the invention, satisfying one or more of the above characteristics.
[0130] Such articles made from composite materials can be used to advantage in many fields.
[0131] The features and advantages of the present invention will be better understood in light of the following examples, which are set forth for illustrative purposes only and do not limit the scope of the invention.
[0132] Comparative Example 1 - Office Paper For example, paper products such as printing and writing paper (Clairfontaine's A4 Clairalpha 80g / m 2 A method for producing carbon fiber using paper is carried out.
[0133] The filler contained in the paper is first removed. To do this, the paper is subjected to the following procedure.
[0134] First, it automatically shreds multiple pieces of paper.
[0135] The resulting fragments are then pretreated to reduce their mineral filler content as well as other impurities. To do this, they are loaded into a pulper with water to form a paper pulp that is suspended in water at 20 g / L dry matter. This pulp is washed three times with pressurized water jets through a 50 μm screen until the water is clear (hyperwash). The hyperwashed pulp is then oven-dried at 95° C. overnight before being crushed to form particles with a size of approximately 250 μm or less.
[0136] Thermogravimetric analysis at different steps of the method determines the mineral filler content of the material and thereby controls its efficiency. For this purpose, a material sample is first exposed in air to a temperature of 500° C. to determine its overall mineral filler content and then in air to a temperature of 900° C. to determine the proportion of carbonates in these mineral fillers.
[0137] In this way, the initial paper is determined to contain 14% mineral filler (made from 94% carbonates) and 5% water. At the end of the pretreatment, the mineral filler content of the ground paper pulp is less than 1%.
[0138] Thereafter, the shredded paper pulp is dissolved in phosphoric acid to an amount of 10% by weight based on the total weight of the mixture.
[0139] To this solution is added an aqueous dispersion of carbon nanotubes, formed by dispersing carbon nanotubes in an amount of 0.9% by weight in water in the presence of a surfactant commercially available as Brij® S20 at a concentration of 1.2% by weight, using a reactor connected to a ball mill and an ultrasonic probe.
[0140] The aqueous dispersion is added to the spinning solution in an amount of 0.1% by weight based on the weight of the ground pulp contained in the spinning solution. The quality of the dissolution is checked by optical microscopy and viscosity measurements. The dispersion does not contain any aggregates with a size of 1 μm or more.
[0141] To this solution is added a non-ionic emulsifier, such as the product sold under the trademark Emran®, in an amount of 0.2% by weight based on the weight of the ground pulp contained in the spinning solution, which is advantageous in facilitating the impregnation of the phosphoric acid into the recycled paper cellulose.
[0142] The mixture is heated to 45° C. for 15 min under a vacuum of 100 mbar with stirring at 40 rpm, then cooled to −10° C. under the same vacuum and stirring for 3 h, then left overnight at 0° C. under the same vacuum and stirring conditions, and finally cooled to −10° C.
[0143] The resulting spinning solution is extruded through a spinneret containing 500 holes each with a diameter of 80 μm and injected directly into a coagulation bath consisting of an isopropanol / water mixture (60:40 by volume).
[0144] The spinning parameters are, for example, a temperature of the spinning solution of 0°C, a speed of the transfer pump of 800 rpm, and a temperature of the coagulation bath of 20°C.
[0145] The carbon nanotubes are captured and well dispersed in a coagulation bath to form cellulose fibers.
[0146] The fibers thus formed are passed through a neutralization bath containing potassium hydroxide, KOH, at 20°C to remove any remaining phosphoric acid from the fibers, and then through a water washing bath at 15°C before being dried with hot air in an oven at 250°C.
[0147] Thereafter, the film is stretched by a conventional method using heated rollers at a temperature of 160°C.
[0148] The cellulosic fibres are then wound onto a spool at a winding speed of 12 m / min.
[0149] This results in a cellulosic multifilament fiber with a diameter of about 25 μm and a length of several meters.
[0150] This continuous cellulosic fiber has a strength of 10 to 40 cN / tex and a Young's modulus of 10 to 30 GPa (these parameters are measured according to the protocol described in the international standard ISO 2062).
[0151] The continuous cellulosic fibers may then undergo a stabilization step in air at a temperature of about 250°C before a carbonization step in nitrogen at up to 1,200°C.
[0152] The method produces carbon fibers that, in the non-graphitized state, have a tensile strength of more than 1,200 MPa and a Young's modulus of more than 75 GPa (these parameters are measured according to the protocol described in Method B of the international standard ISO 11566). EXAMPLES
[0153] Example 1 - Office paper The same paper product as that used in Comparative Example 1 above, printing and writing office paper (Clairfontaine's A4 Clairalpha 80g / m 2 paper) to carry out the method of producing carbon fiber according to the present invention.
[0154] First, multiple pieces of paper are automatically shredded. The resulting pieces are then crushed to form particles with dimensions of approximately 250 μm.
[0155] In accordance with the present invention, the shredded paper is then directly dissolved in an 85% aqueous phosphoric acid solution (containing a phosphoric acid concentration of 85% by volume based on the total volume of the aqueous solution) in an amount of 7% by weight based on the total weight of the mixture to form a spinning solution.
[0156] To this solution is added a non-ionic emulsifier, such as the product sold under the trademark Emran®, in an amount of 0.2% by weight based on the weight of the shredded paper contained in the spinning solution. Such non-ionic emulsifiers are advantageous in facilitating the impregnation of the phosphoric acid into the recycled paper cellulose.
[0157] The mixture is heated to 45° C. for 15 min under a vacuum of 100 mbar with stirring at 40 rpm, then cooled to −10° C. under the same vacuum and stirring for 3 h, then left overnight at 0° C. under the same vacuum and stirring conditions, and finally cooled to −10° C.
[0158] In an alternative embodiment of the method, shredded paper can be mixed into the phosphoric acid solution along with high purity cellulose derived from wood obtained from a papermaking process, for example in a weight ratio of shredded paper to high purity cellulose of 20:80 or 50:50.
[0159] The spinning solution is extruded through a spinneret containing 500 holes, each 80 μm in diameter, and injected directly into a coagulation bath consisting of an isopropanol / water mixture (60:40 by volume).
[0160] The spinning parameters are, for example, a temperature of the spinning solution of 0°C, a speed of the transfer pump of 600 rpm, and a temperature of the coagulation bath of 20°C.
[0161] The cellulose fibers are formed in a coagulation bath.
[0162] To remove any remaining phosphoric acid from the fibers, the fibers thus formed are passed through a neutralization bath containing potassium hydroxide, KOH, at 3% by weight in water at 20°C, and then through a water washing bath at 15°C before being dried with hot air in an oven at 250°C.
[0163] Thereafter, the film is stretched by a conventional method using heated rollers at a temperature of 160°C.
[0164] The cellulosic fibres are then wound onto a spool at a winding speed of 10 m / min.
[0165] This results in a cellulosic multifilament fiber with a diameter of approximately 28 μm and a length of several meters.
[0166] This continuous cellulosic fiber has a strength of 10 to 40 cN / tex and a Young's modulus of 10 to 40 GPa (these parameters are measured according to the protocol described in the international standard ISO 2062).
[0167] The continuous cellulosic fibers may then undergo a stabilization step in air at a temperature of about 250°C before a carbonization step in nitrogen at up to 1,200°C.
[0168] Prior to the carbonization process, the continuous cellulosic fibers can be impregnated with a so-called carbonization agent, which serves to increase the mechanical properties of the final carbon fibers and the carbon yield of the carbonization process.
[0169] The carbonization step can be followed by a graphitization step by heating the fibers in an inert gas at a temperature of 2,000 to 3,000° C. for 1 to 10 minutes.
[0170] The method produces carbon fibers with particularly satisfactory mechanical properties, especially in the non-graphitized state, with a tensile strength of more than 1,200 MPa and a Young's modulus of more than 75 GPa (these parameters are measured according to the protocol described in method B of the international standard ISO 11566). These mechanical properties are as good as those of the carbon fibers obtained in Comparative Example 1, in which a pretreatment was performed before the shredded paper material was dissolved in an aqueous phosphoric acid solution.
[0171] Furthermore, without the addition of any additives, the carbon fibers obtained according to the invention have a carbon yield of 15.4% at 1,000°C in nitrogen and an inorganic content of less than 0.007% (these parameters are measured by thermogravimetric analysis at 10°C / min in nitrogen up to 1,000°C, followed by passage through an air atmosphere at 1,000°C).
[0172] Compared to carbon fibers formed by conventional methods proposed in the prior art, the carbon fibers were obtained at a very low cost.
[0173] The carbon fibers can be used in many applications, for example in the manufacture of composite articles, in which the fibers are dispersed in an organic polymer resin.
[0174] Example 2 - Paper Towels The paper towel is used to carry out the method of producing carbon fiber according to the present invention.
[0175] After the paper is crushed, it is dissolved in phosphoric acid (85% aqueous solution) in an amount of 7% by weight based on the total weight of the mixture.
[0176] To this solution is added a non-ionic emulsifier, such as the product sold under the trademark Emran®, in an amount of 0.2% by weight based on the weight of the ground pulp contained in the spinning dope.
[0177] The mixture is heated to 45° C. under a vacuum of 100 mbar with stirring at 40 rpm for 30 minutes and then cooled to −10° C. under the same vacuum and stirring overnight.
[0178] The resulting spinning solution is extruded through a spinneret containing 500 holes each with a diameter of 80 μm and injected directly into a coagulation bath consisting of an isopropanol / water mixture (60:40 by volume).
[0179] The spinning parameters are, for example, a temperature of the spinning solution of 0°C, a speed of the transfer pump of 600 rpm, and a temperature of the coagulation bath of 20°C.
[0180] The cellulose fibers are formed in a coagulation bath.
[0181] The fibers thus formed are passed through a neutralization bath containing potassium hydroxide KOH at 20°C to remove any remaining phosphoric acid from the fibers, and then through a water washing bath at 15°C before being dried with hot air in an oven at 260°C.
[0182] It is then stretched by a conventional method using heated rollers at a temperature of 120°C.
[0183] These cellulose fibers are then subjected to a carbonization process according to the protocol given in Example 1 above.
Claims
1. A method for producing carbon fibers from a produced paper product, comprising the steps of: a) preparing a cellulosic fiber, comprising the steps of: a1) crushing the paper product to obtain crushed paper material; a3) directly dissolving the ground material obtained at the end of step a1) in an aqueous phosphoric acid solution to form the so-called spinning solution; a4) using the spinning solution to carry out a solvent spinning process to produce continuous cellulosic fibers; and a5) optionally drawing the resulting cellulosic continuous fiber; preparing a cellulosic fiber comprising: b) carbonizing the cellulosic continuous fibers to form carbon fibers; The method according to claim 1, further comprising:
2. 10. The method of claim 1, wherein the spinning solution is subjected to the solvent spinning process without a prior drying step.
3. 3. The method for producing carbon fibers according to claim 1 or 2, wherein the aqueous phosphoric acid solution contains a phosphoric acid concentration of 75 to 99 volume % based on the total volume of the aqueous solution.
4. 4. A method for producing carbon fibers according to claim 1, wherein in step a) of preparing the cellulosic fibers the temperature does not exceed 45°C.
5. 5. A method for producing carbon fibres according to claim 1, wherein in step a1), the crushing is carried out in such a way as to obtain crushed material formed from particles, the largest dimension of which is between 200 and 500 μm.
6. 6. The method for producing carbon fibers according to any one of claims 1 to 5, wherein the paper product is formed from paper originating from chemical paper pulp.
7. 7. The method for producing carbon fibers according to claim 1, wherein in step a3) the crushed material is mixed with purified cellulose.
8. 8. The method for producing carbon fibers according to claim 1, wherein in step a3), the concentration of the crushed material dissolved in the aqueous phosphoric acid solution or the concentration of the mixture of crushed material and purified cellulose is 1 to 50% by weight based on the total weight of the spinning solution.
9. 9. The method of producing carbon fibers according to claim 1, wherein the spinning solution contains a non-ionic emulsifier.
10. 10. A method for producing carbon fibres according to any one of claims 1 to 9, wherein nano-sized carbonaceous fillers, in particular chosen among carbon nanotubes and graphene, alone or mixed, are added to the spinning dope.
11. 11. A method for producing carbon fibers according to any one of claims 1 to 10, comprising forming a web of cellulosic fibers from a plurality of continuous cellulosic fibers obtained in step a4) or a5), wherein step b) of carbonizing the continuous cellulosic fibers is carried out by carbonizing the web of continuous cellulosic fibers to form a carbon fiber based web.
12. 1. A method for producing a composite article containing carbon fibers dispersed in an organic polymer resin matrix, comprising: - carrying out the method for producing carbon fibres according to any one of claims 1 to 10 to form a carbon fibre web from the resulting plurality of said carbon fibres or carrying out the method for producing carbon fibres according to claim 11 to form a carbon fibre-based web, and - manufacturing said article made of composite material from a plurality of the carbon fiber webs thus obtained.
Citation Information
Patent Citations
Method for producing cellulose molded article
JP1997505119A
Method for producing carbon fibers, precursor materials used by the method, and carbon fibers obtained
JP2015537125A
Method for producing carbon fiber woven fabric and carbon fiber woven fabric
JP2016164313A
Process for the production of a cellulose moulded body
US5601767A
Process for making cellulose extrudates
US5804120A