Water-based flame-retardant coating composition and flame-retardant thermoplastic resin film

A water-based flame retardant coating with inorganic phosphate and particles forms a thin, effective flame-retardant layer on thermoplastic resin films, addressing environmental risks and maintaining mechanical strength while achieving high flame retardancy.

JP7593996B2Active Publication Date: 2024-12-03株式会社ユポ

Patent Information

Application Number
JP2022509420
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-03-27
Filing Date
2021-02-19
Publication Date
2024-12-03
Estimated Expiration
2041-02-19

AI Technical Summary

Technical Problem

Conventional halogen-based flame retardants pose environmental and health risks, and non-halogen alternatives require large amounts, impacting mechanical strength and increasing costs, while existing non-halogen flame retardant compositions impair base material properties when thickly coated.

Method used

A water-based flame retardant coating composition containing inorganic phosphate, inorganic particles, and a water-based binder resin is applied thinly, forming a flame-retardant thermoplastic resin film that maintains base material properties and achieves excellent flame retardancy.

Benefits of technology

The composition provides excellent flame retardancy without impairing the base material's properties, allowing for thin coatings that are cost-effective and maintain the film's characteristics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007593996000001
    Figure 0007593996000001
Patent Text Reader

Abstract

The present invention pertains to an aqueous flame-retardant coating composition that contains: an inorganic phosphate; inorganic particles; an aqueous binder resin that can be dissolved or dispersed in water; and water. With respect to 100 parts by mass of the total of the inorganic phosphate and the inorganic particles, the contained amount of the aqueous binder resin is 3-60 parts by mass.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a water-based flame-retardant coating composition and a flame-retardant thermoplastic resin film. [Background technology]

[0002] Halogen-containing flame retardants have been used in the past because they have a flame-retardant effect and are relatively good in moldability and mechanical strength. However, halogen-containing flame retardants may generate halogen gases during processing or combustion, which may have adverse effects on the human body and the environment, and may cause corrosion of metals.

[0003] As a non-halogen flame retardant that does not contain halogen, phosphorus-based flame retardants are listed, and various flame-retardant resin compositions in which phosphorus-based flame retardants are combined with polyolefin resins, nitrogen-containing resins, graphite, etc. have been investigated. Patent Document 1 discloses a flame-retardant resin composition containing a thermoplastic resin, a layered silicate, and a non-halogen flame retardant, and lists a phosphorus-based compound as the non-halogen flame retardant.

[0004] However, in order to achieve sufficient flame retardancy, the flame-retardant resin composition disclosed in Patent Document 1 requires a large amount of flame retardant to be kneaded into the base material, which raises concerns about a decrease in moldability and mechanical strength of the flame-retardant resin composition.

[0005] Therefore, Patent Document 2 discloses a flame retardant composition comprising an organic resin component, an ammonium salt of inorganic phosphoric acid, and a layered inorganic material. Attempts have been made to impart flame retardant properties to a fiber sheet by coating the flame retardant composition on the fiber sheet and drying it. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Japanese Patent Application Publication No. 2003-171569 [Patent Document 2] Japanese Patent Publication No. 2007-246697 Summary of the Invention [Problem to be solved by the invention]

[0007] However, in order to achieve good flame retardancy, it is necessary to apply a thick coating of the flame retardant composition to the surface of the fiber sheet, which may impair the inherent properties of the substrate such as the fiber sheet, as in the case of kneading or impregnation, and there is also a concern of an increase in costs due to the use of a large amount.

[0008] Therefore, the present invention aims to provide a flame-retardant coating composition that does not contain halogens, can be applied thinly to the surface of a substrate, and can impart excellent flame retardancy, and a flame-retardant thermoplastic resin film having a layer formed from such a flame-retardant coating composition. [Means for solving the problem]

[0009] As a result of extensive research, the present inventors have found that by using an aqueous flame-retardant coating composition containing inorganic phosphate, inorganic particles, an aqueous binder resin and water in specific ratios, it is possible to apply a thin coating that does not impair the properties of the substrate and also to impart excellent flame retardancy, and have thus completed the present invention.

[0010] That is, the present invention relates to the following [1] to

[12] . [1] An aqueous flame-retardant coating composition comprising an inorganic phosphate, inorganic particles, an aqueous binder resin that is soluble or dispersible in water, and water, wherein the content of the aqueous binder resin is 3 to 60 parts by mass per 100 parts by mass of the total of the inorganic phosphate and the inorganic particles. [2] The aqueous flame-retardant coating composition according to [1] above, wherein a mass ratio of the inorganic phosphate to the inorganic particles is 95:5 to 50:50. [3] The aqueous flame-retardant coating composition according to [1] or [2] above, wherein the inorganic phosphate comprises ammonium polyphosphate. [4] The aqueous flame-retardant coating composition according to any one of the above [1] to [3], wherein the inorganic particles contain a layered silicate. [5] The aqueous flame-retardant coating composition according to any one of the above [1] to [4], wherein the aqueous binder resin is crosslinked with at least one crosslinking agent selected from the group consisting of a metal crosslinking agent, an epoxy crosslinking agent, an epichlorohydrin crosslinking agent, and an oxazoline crosslinking agent. [6] The aqueous flame-retardant coating composition according to any one of the above [1] to [5], wherein the aqueous binder resin comprises an acrylic resin, and the acrylic resin is dispersed in the aqueous flame-retardant coating composition. [7] A flame-retardant thermoplastic resin film, comprising a layer formed on at least one surface of the thermoplastic resin film from the aqueous flame-retardant coating composition according to any one of [1] to [6] above.

[0011] [8] A flame-retardant thermoplastic resin film comprising a flame-retardant layer on at least one surface of the thermoplastic resin film, the flame-retardant layer containing inorganic phosphate, inorganic particles, and an aqueous binder resin that is soluble or dispersible in water, wherein the content of the aqueous binder resin is 3 to 60 parts by mass per 100 parts by mass of the total of the inorganic phosphate and the inorganic particles. [9] The flame-retardant thermoplastic resin film according to [8], wherein a mass ratio of the inorganic phosphate to the inorganic particles is 95:5 to 50:50.

[10] 100 g / m of the resin component of the thermoplastic resin film 2 The inorganic phosphate in the flame-retardant layer is 1 to 45 g / m 2 and the inorganic particles are 0.1 to 25 g / m 2 The flame-retardant thermoplastic resin film according to [8] or [9] above.

[11] 100 g / m of the resin component of the thermoplastic resin film 2 whereas the total amount of the inorganic phosphate and the inorganic particles in the flame-retardant layer is 50 g / m 2 The flame-retardant thermoplastic resin film according to any one of the above [8] to

[10] , wherein the flame-retardant thermoplastic resin film has a viscosity of less than 100%.

[12] The flame-retardant thermoplastic resin film according to any one of [8] to

[11] , further comprising at least one of a printing layer and a print-receiving layer on the surface of the flame-retardant layer opposite to the side on which the thermoplastic resin film is located. Effect of the Invention

[0012] The aqueous flame-retardant coating composition according to the present invention has excellent coatability and flame retardancy, and therefore exhibits excellent flame retardancy even when applied thinly to the surface of a substrate. Therefore, it is possible to impart good flame retardancy at low cost without impairing the properties of the substrate. A flame-retardant thermoplastic resin film having a layer formed from such an aqueous flame-retardant coating composition exhibits excellent flame retardancy, and at the same time, the inherent properties of the thermoplastic resin film are not suppressed and are expressed. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The present invention will be described in detail below, but the present invention is not limited to the following embodiments and can be modified in any manner without departing from the gist of the present invention.

[0014] <Water-based flame-retardant paint composition> The aqueous flame-retardant coating composition according to the present embodiment (hereinafter, sometimes simply referred to as the "coating composition") contains an inorganic phosphate, inorganic particles, an aqueous binder resin that is soluble or dispersible in water, and water. The content of the aqueous binder resin is 3 to 60 parts by mass per 100 parts by mass of the total of the inorganic phosphate and the inorganic particles.

[0015] (Inorganic Phosphates) Inorganic phosphates are components that function mainly as flame retardants in coating compositions. The phosphoric acid in "inorganic phosphates" includes orthophosphoric acid, phosphorous acid, hypophosphorous acid, polyphosphoric acid, etc., and is preferably orthophosphoric acid. Inorganic phosphates form an incombustible carbonized layer called char through a dehydration carbonization reaction caused by a strong acid generated during combustion. On the other hand, inorganic phosphates also have a radical trapping effect in the gas phase. Inorganic phosphates function as flame retardants, particularly by insulating the substrate from heat and oxygen through the carbonized layer.

[0016] The inorganic phosphate is not particularly limited as long as it is a salt that performs the above-mentioned function, and examples thereof include ammonium salts of inorganic phosphoric acid and metal salts of inorganic phosphoric acid. These inorganic phosphates may be used alone or in combination. From the viewpoint of the effects of the present invention, the inorganic phosphate is more preferably ammonium salts of inorganic phosphoric acid.

[0017] In the case of inorganic ammonium salt of phosphoric acid, when the temperature reaches the decomposition temperature by heating accompanying combustion, ammonia is released to form condensed phosphoric acid. This condensed phosphoric acid acts as a dehydrating solvent to form the carbonized layer. The ammonia gas generated at the same time acts as a foaming agent and has the function of expanding the coating composition.

[0018] Examples of ammonium salts of inorganic phosphoric acid include monoammonium phosphate, diammonium phosphate, triammonium phosphate, ammonium phosphite, ammonium hypophosphite, ammonium polyphosphate, etc. Among these, ammonium polyphosphate is preferred from the viewpoint of water resistance of the coating film.

[0019] In the case of metal salts of inorganic phosphates, they act as dehydration catalysts and also function to form a non-flammable inorganic phosphate coating. Examples of metal salts of inorganic phosphoric acid include sodium salts such as monosodium phosphate, disodium phosphate, trisodium phosphate, monosodium phosphite, disodium phosphite, and sodium hypophosphite; potassium salts such as monopotassium phosphate, dipotassium phosphate, tripotassium phosphate, monopotassium phosphite, dipotassium phosphite, and potassium hypophosphite; lithium salts such as monolithium phosphate, dilithium phosphate, trilithium phosphate, monolithium phosphite, dilithium phosphite, and lithium hypophosphite; barium salts such as barium dihydrogen phosphate, barium hydrogen phosphate, tribarium phosphate, and barium hypophosphite; magnesium salts such as monohydrogen magnesium phosphate, dihydrogen magnesium phosphate, trimagnesium phosphate, and magnesium hypophosphite; calcium salts such as calcium dihydrogen phosphate, calcium hydrogen phosphate, tricalcium phosphate, and calcium hypophosphite; zinc salts such as zinc phosphate, zinc phosphite, and zinc hypophosphite; and aluminum salts such as aluminum phosphate, aluminum phosphite, and aluminum hypophosphite. Among these, aluminum phosphite is preferred because it exhibits high flame retardancy by forming an oxide film.

[0020] When ammonium polyphosphate is used as the inorganic phosphate, the ammonium polyphosphate may be manufactured or commercially available, such as EXOLIT AP 423 (trade name) and AP462 (trade name) manufactured by Clariant, Sumisafe P (trade name) manufactured by Sumitomo Chemical Co., Ltd., and Terrage C60 (trade name) manufactured by Chisso Corporation.

[0021] The inorganic phosphate has an average primary particle size of preferably 0.5 μm or more, more preferably 3.0 μm or more, and even more preferably 5.0 μm or more in terms of suppressing an increase in the viscosity of the paint, and an average primary particle size of preferably 35 μm or less, more preferably 25 μm or less, and even more preferably 15 μm or less in terms of particle dispersibility and flame retardancy, i.e., a smaller particle size increases the specific surface area and improves flame retardancy. In this specification, the average primary particle size of the inorganic phosphate is the volume average particle size measured using a laser diffraction particle size distribution measuring device (SALD-2200, manufactured by Shimadzu Corporation), and refers to the median diameter represented by D50.

[0022] The content of the inorganic phosphate in the coating composition is preferably 50 parts by mass or more, more preferably 55 parts by mass or more, and even more preferably 70 parts by mass or more, based on 100 parts by mass of the total of the inorganic phosphate and the inorganic particles, in order to sufficiently form a carbonized foam layer and to exhibit flame retardancy. The content of the inorganic phosphate is preferably 95 parts by mass or less, more preferably 85 parts by mass or less, and even more preferably 78 parts by mass or less, in order to prevent the inorganic phosphate from falling off from the flame retardant layer and to exhibit sufficient flame retardancy.

[0023] (Inorganic particles) The inorganic particles are not particularly limited as long as they form a non-flammable gas or an inorganic layer when heated by combustion. Examples of such materials include layered silicates, titanium oxide, silica, boric acid, zinc borate, lead borate, sodium borate (borax), expandable graphite, calcium carbonate, magnesium carbonate, glass (hollow glass beads), shirasu (silas balloons), zinc oxide, zirconium oxide, alumina, silica alumina, magnesia, zeolite, aluminum hydroxide, magnesium hydroxide, etc. One or more of these materials may be used.

[0024] Among inorganic particles, layered silicates are preferred from the viewpoint of the effect of blocking flammable gases generated during combustion. Examples of layered silicates include smectite clay minerals such as montmorillonite, saponite, hectorite, beidellite, stevensite, and nontronite, as well as talc, kaolinite, pyrophyllite, vermiculite, halloysite, and swelling mica. Among the above, smectite clay minerals can incorporate a large amount of water between the crystal layers, and when heated by combustion, the water incorporated between the layers volatilizes, cooling the thermoplastic resin, and the volatilized water reduces the surrounding oxygen concentration. As a result, the effect of further improving flame retardancy is high, so smectite clay minerals are more preferred. Among the smectite clay minerals, montmorillonite and beidellite are even more preferred.

[0025] The average primary particle size of the inorganic particles is preferably 0.01 μm or more, more preferably 0.05 μm or more, and even more preferably 0.1 μm or more, in order to suppress an increase in the viscosity of the coating material. salt The particles are smaller than inorganic phosphate. salt The inorganic particles enter the gaps between the particles. This forms a dense layer, which can block the flow of flammable gas and further improve the flame retardancy, which is preferable. Specifically, the average primary particle size of the inorganic particles is preferably 10 μm or less, more preferably 8 μm or less, and even more preferably 6 μm or less. In this specification, the average primary particle size of inorganic particles refers to the volume average particle size measured using a laser diffraction particle size distribution measuring device (SALD-2200, manufactured by Shimadzu Corporation), and refers to the median diameter represented by D50.

[0026] The content of inorganic particles in the coating composition is preferably 5 parts by mass or more, more preferably 15 parts by mass or more, and even more preferably 22 parts by mass or more, because flame retardancy decreases when the content is below the lower limit relative to 100 parts by mass of the total of inorganic phosphate and inorganic particles, that is, there is a risk of a decrease in water content and insufficient blocking of flammable gas. Also, the content of inorganic particles is preferably 50 parts by mass or less, more preferably 45 parts by mass or less, and even more preferably 30 parts by mass or less, in order to suppress an increase in viscosity of the coating.

[0027] That is, the ratio of the contents (mass ratio) represented by inorganic phosphate:inorganic particles is preferably 95:5 to 50:50, more preferably 85:15 to 55:45, further preferably 85:15 to 70:30 or 78:22 to 55:45, and even more preferably 78:22 to 70:30. The content ratio of 95:5 to 50:50 means that the content ratio of the inorganic particles to the total content of the inorganic phosphate and the inorganic particles is 0.05 to 0.5. The content ratio of inorganic particles is preferably 0.05 or more to ensure sufficient water content and good flame retardancy by blocking flammable gases, and is preferably 0.5 or less to suppress an increase in the viscosity of the paint.

[0028] (Water-based binder resin) The aqueous binder resin means a resin that is soluble or dispersible in water. Since the coating composition also contains water, when the aqueous binder resin dissolves in the water contained in the coating composition, the aqueous binder resin is contained as an aqueous solution. When the aqueous binder resin does not dissolve in the water contained in the coating composition, the aqueous binder resin is dispersed in water, that is, contained as an emulsion. From the viewpoint of water resistance, the aqueous binder resin is preferably contained as an emulsion. In this specification, "dispersed" means that the resin particles are present in a uniform and stable state in the solvent.

[0029] The content of the aqueous binder resin in the coating composition is 3 parts by mass or more, preferably 5 parts by mass or more, and more preferably 10 parts by mass or more, based on 100 parts by mass of the total of the inorganic phosphate and the inorganic particles, from the viewpoint of obtaining good surface strength when formed into a coating film. Also, the content of the aqueous binder resin is 60 parts by mass or less, preferably 45 parts by mass or less, and more preferably 30 parts by mass or less, from the viewpoint of obtaining good flame retardancy.

[0030] Examples of the water-dispersible aqueous binder resin include acrylic resin, urethane resin, fluororesin, polystyrene resin, vinyl chloride resin, etc. These resins may be used alone or in combination with two or more other types of aqueous binder resins that are soluble in water. These resins may be modified with other resin components, and may be partially crosslinked with a crosslinking agent.

[0031] Among these, acrylic resins are preferred from the viewpoints of weather resistance and ease of handling, and it is more preferred that the acrylic resin is dispersed in the coating composition. In this specification, the acrylic resin means a polymer of at least one (meth)acrylic monomer selected from the group consisting of (meth)acrylic acid monomers and (meth)acrylic acid ester monomers, and may be a copolymer of a (meth)acrylic monomer and another monomer. Here, the (meth)acrylic acid refers to at least one of acrylic acid and methacrylic acid. Among the acrylic resins, styrene acrylic resin is particularly preferred.

[0032] From the viewpoint of flexibility, the water-dispersible aqueous binder resin is preferably a thermoplastic resin.

[0033] Examples of the water-soluble aqueous binder resin include acrylic resin, silicone resin, acrylic silicone resin, fluororesin, epoxy resin, vinyl resin, phenol resin, urethane resin, melamine resin, ketone resin, etc. These resins may be used alone or in combination of two or more.

[0034] Among these, acrylic resins are preferred from the viewpoints of weather resistance and ease of handling, and thermoplastic resins are preferred from the viewpoint of flexibility. These resins may be modified with other resin components, and may be partially crosslinked with a crosslinking agent.

[0035] The type of crosslinking agent is not particularly limited, but crosslinking with at least one crosslinking agent selected from the group consisting of metal-based crosslinking agents, epoxy-based crosslinking agents, epichlorohydrin-based crosslinking agents, and oxazoline-based crosslinking agents is preferred from the viewpoint of water resistance of the coating film. Examples of the metal crosslinking agent include ammonium zirconium carbonate, sodium zirconium carbonate, zinc sulfate, etc., and ammonium zirconium carbonate is preferred from the viewpoint of water resistance.

[0036] The content of the crosslinking agent varies depending on the crosslinking agent used, but for example, when a metal-based crosslinking agent is used, the content of the metal-based crosslinking agent is preferably 0.04 parts by mass or more, more preferably 0.2 parts by mass or more, and even more preferably 0.4 parts by mass or more, relative to 100 parts by mass of the total content of the aqueous binder resin, in order to exhibit the crosslinking effect well. Also, from the viewpoint of the viscosity of the paint and the flexibility of the coating film, the content is preferably 32 parts by mass or less, more preferably 16 parts by mass or less, and even more preferably 8 parts by mass or less.

[0037] (Solvent or Dispersion Medium) The coating composition contains water as a solvent or dispersion medium, but may further contain a solvent or dispersion medium other than water. Water is preferable from the viewpoints of the effect on the environment and human body and cost, and ion-exchanged water is more preferable. Examples of the solvent or dispersion medium other than water include alcohols such as ethanol and 2-propanol.

[0038] The content of water in the coating composition relative to the total amount of the solvent and the dispersion medium is preferably 50% by mass or more, more preferably 90% by mass or more, and even more preferably 100% by mass. The water is preferably ion-exchanged water.

[0039] The solid content of the coating composition is preferably 3% by mass or more, more preferably 5% by mass or more, and even more preferably 8% by mass or more, and is preferably 30% by mass or less, more preferably 25% by mass or less, and even more preferably 20% by mass or less. The solids concentration of the coating composition was determined by precisely weighing 1.0 g of the coating composition into an aluminum cup, drying this in an oven at 120°C for 30 minutes, and then precisely weighing the mass of the residue. The ratio of the mass of the residue to the original mass was calculated as the heating residue (mass%). The solids concentration of the coating composition can be adjusted by the total content of the solvent and the dispersion medium.

[0040] (optional ingredient) In addition to the above components, the coating composition may contain other optional components as long as the effects of the present invention are not impaired. Examples of other optional components include silane coupling agents, pigments, wetting agents, dispersants, emulsifiers, thickeners, anti-settling agents, anti-skinning agents, anti-sagging agents, defoamers, color separation inhibitors, leveling agents, drying agents, plasticizers, rust inhibitors, antibacterial agents, insecticides, preservatives, light stabilizers, ultraviolet absorbers, antistatic agents, conductivity imparting agents, etc. These can be used as known agents in known methods.

[0041] (Coating method) The coating composition can be prepared by mixing the inorganic phosphate, inorganic particles, a water-based binder resin, water and other optional components. The obtained coating composition is applied to at least one surface of the substrate to be coated, and then dried to obtain a coating film. The coating film of the coating composition may be formed on one surface of the substrate, or on both surfaces. From the viewpoint of the flame retardancy of the flame-retardant thermoplastic resin film, it is preferable to form the coating film on both surfaces of the substrate. When the coating film is formed on both sides, the configuration of the coating film on both sides may be the same or different, and the thickness may be the same or different.

[0042] The coating film is formed by volatilization of a solvent such as water in the coating composition, and becomes a flame-retardant layer containing inorganic phosphate, inorganic particles, and an aqueous binder resin that is soluble or dispersible in water.

[0043] The substrate to which the coating composition according to the present embodiment is applied is not particularly limited, and examples thereof include thermoplastic resin films, thermosetting resin films, nonwoven fabrics, paper, glass, etc. Among these, thermoplastic resin films are preferred because they can more significantly exhibit the superiority of the coating composition according to the present embodiment, that is, high flame retardancy at a thin film thickness. The thermoplastic resin constituting the thermoplastic resin film is not particularly limited, and examples thereof include polyethylene resin, polypropylene resin, polyester resin, polyamide resin, polystyrene resin, polyethylene terephthalate resin, polyvinyl chloride resin, polycarbonate resin, etc. These may be used alone or in combination of two or more.

[0044] The coating composition can be applied to any of the above substrates. However, when the substrate is a thermoplastic resin film, for example, the suitable coating amount of the coating composition varies depending on the oxygen index of the thermoplastic resin that constitutes the film. The oxygen index is the minimum oxygen concentration in a mixed gas of oxygen and nitrogen required for a resin to maintain flaming combustion. The smaller the oxygen index, the easier the resin will burn, and the larger the oxygen index, the harder it will burn.

[0045] Among the thermoplastic resins constituting the thermoplastic resin film given above as examples, resins having an oxygen index of less than 20 include, for example, polyethylene resin, polypropylene resin, polystyrene resin, and the like. On the other hand, examples of resins having an oxygen index of 20 or more include polyethylene terephthalate resin, polyvinyl chloride resin, polyamide resin, etc. In addition, the "oxygen index" in this specification is the value described in "Plastics, 44(9), 18, 1993 (Polymer Data Book, p. 91)".

[0046] Thermoplastic resins with an oxygen index of less than 20 are more combustible than thermoplastic resins with an oxygen index of 20 or more, and are therefore more preferred in that the flame retardant effect of the coating composition according to this embodiment is more pronounced. Among these, polyethylene resins and polypropylene resins, which have low oxygen indexes and are generally considered difficult to make flame retardant, are even more preferred. On the other hand, a thermoplastic resin with an oxygen index of 20 or more is preferably used because it is inherently less flammable than a thermoplastic resin with an oxygen index of less than 20, and therefore even if the coating amount of the coating composition according to this embodiment is small, it will become a flame-retardant thermoplastic resin film that is less flammable. Polyethylene terephthalate resin and polyamide resin are even more preferred.

[0047] The coating composition can impart high flame retardancy to a substrate with a smaller amount of coating than conventional coating compositions, regardless of the oxygen index of the thermoplastic resin film. When forming a coating film of the coating composition on a thermoplastic resin film, the coating amount is 100 g / m 2 The total coating weight of inorganic phosphate and inorganic particles is 50g / m 2 Even if the amount is less than this, sufficient flame retardancy can be imparted. If the oxygen index of the thermoplastic resin film is less than 20, the resin content of the thermoplastic resin film is 100 g / m 2 The total coating weight of inorganic phosphate and inorganic particles is 50g / m 2 Less than 40 g / m is more preferable. 2 More preferably, the total coating weight of the inorganic phosphate and inorganic particles is 15 g / m or less. 2 More preferably, 25 g / m 2 The above is even more preferable. On the other hand, when the oxygen index of the thermoplastic resin film is 20 or more, high flame retardancy can be achieved with a flame-retardant layer having a smaller thickness. 2 The total coating weight of inorganic phosphate and inorganic particles is 20g / m 2 Less than 10 g / m is more preferable. 2 More preferably, the total coating amount of the inorganic phosphate and the inorganic particles is 0.5 g / m or less. 2 More preferably, 2 g / m 2 The above is even more preferable. By setting the total coating amount of the inorganic phosphate and the inorganic particles to the above upper limit or less, the productivity of the obtained flame-retardant thermoplastic resin film can be ensured and an increase in cost can be suppressed, while by setting it to the above lower limit or more, the fire spread time of the obtained flame-retardant thermoplastic resin film can be shortened. The ratio (mass ratio) of the contents of the inorganic phosphate and the inorganic particles contained in the flame-retardant layer, and the content of the aqueous binder resin per 100 parts by mass of the total of the inorganic phosphate and the inorganic particles, are as described above.

[0048] When the substrate is a thermoplastic resin film, the thickness is preferably 50 μm or more, more preferably 60 μm or more, and even more preferably 70 μm or more from the viewpoint of obtaining good film strength, and is preferably 300 μm or less, more preferably 200 μm or less, and even more preferably 100 μm or less from the viewpoint of obtaining good flexibility.

[0049] <Flame-retardant thermoplastic resin film> The flame-retardant thermoplastic resin film according to this embodiment includes a flame-retardant layer on at least one surface of the thermoplastic resin film, the flame-retardant layer containing an inorganic phosphate, inorganic particles, and an aqueous binder resin that is soluble or dispersible in water. The content of the aqueous binder resin is 3 to 60 parts by mass relative to 100 parts by mass in total of the inorganic phosphate and the inorganic particles.

[0050] Preferred aspects of the inorganic phosphate, inorganic particles, and water-soluble or dispersible aqueous binder resin constituting the flame-retardant layer, as well as the thermoplastic resin film, are the same as the preferred aspects described above in the <Water-based flame-retardant coating composition>.

[0051] When flame-retardant layers are formed on both surfaces of a thermoplastic resin film, the flame-retardant layers on both surfaces may have the same or different configurations and may have the same or different thicknesses. Furthermore, when flame-retardant layers are formed on both surfaces, the preferred contents and coating amounts of the inorganic phosphate, inorganic particles, and aqueous binder resin constituting the flame-retardant layers are such that the total contents and coating amounts of the inorganic phosphate, inorganic particles, and aqueous binder resin constituting the flame-retardant layers on both surfaces are the preferred contents and coating amounts described in the above <Water-based flame-retardant coating composition>.

[0052] The flame-retardant thermoplastic resin film may also be provided with at least one of a printing layer and a print-receiving layer on the surface of the flame-retardant layer opposite to the side on which the thermoplastic resin film is located.

[0053] The printed layer is a layer consisting of characters, images, etc. formed with printing ink or toner, and various printing methods can be used, such as offset printing, inkjet method, electrophotographic (laser) method, thermal recording method, thermal transfer method, etc. Therefore, the printed layer is located on the outermost surface of the flame-retardant thermoplastic resin film, and it is sufficient that the printed layer covers at least a part of the surface area of ​​the flame-retardant thermoplastic resin film, or it may cover the entire area. The printing layer may be a conventionally known one, and may be formed by a known method.

[0054] The print-receiving layer is a layer that functions as an ink or toner-receiving layer when a print layer is provided. Depending on the properties of the print-receiving layer, the various properties of the print layer, such as abrasion resistance, antistatic property, printability, water resistance, storage stability, etc., can be adjusted. The print-receiving layer may be a conventionally known layer using a known method.

[0055] In addition to the print layer and the print-receiving layer, the flame-retardant thermoplastic resin film may have any other layer provided that the effect of the present invention is not impaired. Examples of the other optional layers include a pressure-sensitive adhesive layer, a gloss layer, and a gas barrier layer.

[0056] <Physical properties of water-based flame-retardant paint composition> (Flame retardancy: UL94 VTM test) To evaluate the flame retardancy of the aqueous flame-retardant coating composition, the following tests are carried out using a flame-retardant thermoplastic resin film having a substrate of a thermoplastic resin film, both surfaces of which have been coated with the aqueous flame-retardant coating composition and dried to form a flame-retardant layer. Cut the flame-retardant thermoplastic resin film into a sheet of 50 mm x 200 mm, mark the sheet with a mark 125 mm from the bottom end of the long side, and then leave it to condition for 48 hours or more under conditions of 23°C and 50% relative humidity. Cellophane tape (registered trademark) is applied to the long sides of the sheet within a range of 125 to 200 mm from the bottom end, and the short sides are rolled and glued so that the diameter is 13 mm, to form the sheet into a cylindrical shape. The upper end of the cylindrical sheet is clamped and hung, and 0.05 g or less of cotton (100%) is placed 300 mm below the lower end. A burner with a diameter of 10 mm is prepared and adjusted so that the gas flow rate is 105 mL / min and the blue flame is 20 mm high. The burner is positioned between the cylindrical sheet and the cotton, and the bottom end of the cylindrical sheet is brought into contact with the blue flame at a position 10 mm high, and the flame is applied twice for 3 seconds. This operation is used to check whether the cylindrical sheet melts up to the marked line and whether the cotton (100%) is burned due to ignition caused by the molten sheet falling. It is preferable that the cylindrical sheet does not melt up to the marked line, and it is even more preferable that the cotton does not burn.

[0057] (Flame retardancy: fire spread time) As in the UL94 VTM test, a flame is applied to a cylindrical sheet of flame-retardant thermoplastic resin film for 3 seconds, and the time it takes for the fire to go out is measured. The time it takes for the fire to go out is preferably less than 20 seconds, and more preferably less than 15 seconds.

[0058] (Coatability) In order to evaluate the coatability of the aqueous flame retardant coating composition, an aqueous dispersion is prepared by adjusting the amount of water so that the solid content of the aqueous flame retardant coating composition is 10% by weight. The viscosity of the aqueous dispersion is measured at a rotor speed of 60 rpm and 20°C using a B-type viscometer. From the viewpoint of stable coating with a small coating amount and obtaining a good coating film, the viscosity is preferably 8000 mPa·s or less, more preferably 1500 mPa·s or less, and even more preferably 500 mPa·s or less. In addition, from the viewpoint of suppressing the generation of aggregates due to precipitation of inorganic phosphates, etc., the viscosity is preferably 5 mPa·s or more, more preferably 50 mPa·s or more, and even more preferably 100 mPa·s or more.

[0059] (Surface strength) The surface strength of the flame-retardant layer formed using the water-based flame-retardant coating composition is evaluated by the following test. A 5 cm long piece of Cellophane Tape (registered trademark) manufactured by Nichiban Co., Ltd. is applied to the surface of the flame retardant layer, and then 2.5 cm is peeled off by hand at a low speed (2.5 cm / s) and the remaining 2.5 cm is peeled off at a high speed (25 cm / s). The surface strength is evaluated based on the degree of peeling of the flame retardant layer after peeling. It is preferable that the peeled area when peeled off at high speed and low speed is small. EXAMPLES

[0060] The present invention will be described in more detail below with reference to examples, comparative examples, and test examples. The materials, amounts, ratios, operations, etc. shown in the following examples can be changed as appropriate without departing from the spirit of the present invention. Therefore, the scope of the present invention is not limited to the specific examples shown below. In addition, % described below means % by mass unless otherwise specified.

[0061] [Example 1] Inorganic phosphate (ammonium polyphosphate, Clariant Chemicals, EXOLIT AP 423, average primary particle size D50 = 10 μm) 75 parts by mass, inorganic particles (purified bentonite, Kunimine Industries, Kunipia-F, average primary particle size D50 = 2 μm) 25 parts by mass, water-based binder resin (styrene acrylic resin, Seiko PMC, Hi-Loss X ZE-1425, solid content concentration 48% by mass) 25 parts by mass (solid content equivalent), crosslinker (ammonium zirconium carbonate, San Nopco, 5800MT) 1 part by mass were mixed, and ion-exchanged water was added to a solid content concentration of 10% by mass to obtain a water-based flame-retardant paint composition. Note that bentonite is inorganic particles mainly composed of montmorillonite. The obtained water-based flame-retardant paint composition was applied to both sides of a thermoplastic resin film (polypropylene synthetic paper, porous biaxially oriented film, Yupo Corporation, FPG80, thickness 80 μm) in a coating amount of 5 g / m2 in terms of solid content. 2 The coating was then dried at 80°C for 10 minutes to form a flame-retardant layer, yielding a flame-retardant thermoplastic resin film. Resin component of flame-retardant thermoplastic resin film 100g / m 2 The contents of inorganic phosphate and inorganic particles relative to the total weight are as shown in Table 1. The solids concentration of the paint composition was determined by precisely weighing 1.0 g of the paint composition into an aluminum cup, drying it in an oven at 120°C for 30 minutes, and then precisely weighing the mass of the residue. The ratio of the mass of the residue to the original mass was calculated as the heating residue (mass%).

[0062] [Examples 2 to 6 and Comparative Examples 1 to 3] Each of the flame-retardant thermoplastic resin films of Examples 2 to 6 and Comparative Examples 1 to 3 was obtained in the same manner as in Example 1, except that the compounding ratios of the inorganic phosphate, inorganic particles, and aqueous binder resin, and the coating amount of the aqueous flame-retardant coating composition were changed to the values ​​shown in Table 1. In Table 1, "-" in the column for the aqueous flame-retardant coating composition means that it is not contained.

[0063] [Examples 7 and 8] The flame-retardant thermoplastic resin films of Examples 7 and 8 were obtained in the same manner as in Example 1, except that a thermoplastic resin film (polypropylene-based synthetic paper, porous biaxially oriented film, manufactured by Yupo Corporation, FPG130, thickness 130 μm) was used and the coating amount of the water-based flame-retardant coating composition was changed to the value shown in Table 1.

[0064] [Example 9] A flame-retardant thermoplastic resin film was obtained in the same manner as in Example 1, except that a thermoplastic resin film (polypropylene-based synthetic paper, porous biaxially oriented film, manufactured by Yupo Corporation, FPG200, thickness 200 μm) was used and the coating amount of the water-based flame-retardant coating composition was changed to the value shown in Table 1.

[0065] [Example 10] A flame-retardant thermoplastic resin film was obtained in the same manner as in Example 1, except that a thermoplastic resin film (polypropylene-based synthetic paper, porous biaxially oriented film, manufactured by Yupo Corporation, FPG250, thickness 250 μm) was used and the coating amount of the water-based flame-retardant coating composition was changed to the value shown in Table 1.

[0066] [Example 11] A flame-retardant thermoplastic resin film was obtained in the same manner as in Example 1, except that a thermoplastic resin film (polyethylene terephthalate, biaxially oriented film, Mitsubishi Gas Chemical Company, Diafoil O-100E, thickness 100 μm) was used and the coating amount of the water-based flame-retardant coating composition was changed to the value shown in Table 1.

[0067] [Examples 12 to 15 and Comparative Examples 4 and 5] A flame-retardant thermoplastic resin film was obtained in the same manner as in Example 1, except that the blending amount of the aqueous binder resin and the coating amount of the aqueous flame-retardant coating composition were changed to the values ​​shown in Table 1.

[0068] [Comparative Example 6] A flame-retardant thermoplastic resin film was obtained in the same manner as in Example 11, except that the compounding ratios and coating amounts of the inorganic phosphate, inorganic particles, and aqueous binder resin were changed to the values ​​shown in Table 1.

[0069] [Comparative Example 7] Instead of the aqueous flame-retardant coating composition of Example 1, an organic phosphate (a compound containing an ester structure of pentaerythritol and two phosphoric acids in the main skeleton, manufactured by Teijin Ltd., Fireguard FCX210, average primary particle size D50 = 20 μm), colloidal silica as inorganic particles, and a mixed emulsion of a styrene acrylic acid ester copolymer and a polyester resin as an aqueous binder resin were used, and a flame-retardant thermoplastic resin film was obtained in the same manner as in claim 1, except that the coating amount in solid content conversion shown in Table 1 was used. Note that the "*" in the compounding ratio of the inorganic phosphate in Table 1 means that although it is an organic phosphate, the compounding ratio is listed in the item for convenience.

[0070] The flame-retardant thermoplastic resin film obtained was evaluated as follows. The results are shown in Table 1. In the coatability evaluation, the numerical value indicates the viscosity, the values ​​in parentheses indicate the evaluations A to D, and "-" indicates that the evaluation was not performed.

[0071] (Flame retardancy: UL94 VTM test) The flame-retardant thermoplastic resin film was cut into a sheet of 50 mm x 200 mm, and a mark was drawn 125 mm from the bottom end of the long side of the sheet. The sheet was then left to stand for 48 hours or more under conditions of 23°C and a relative humidity of 50% for conditioning. Cellophane tape (registered trademark) was applied to the long sides of the sheet within a range of 125 to 200 mm from the bottom end, and the short sides were rounded and glued to a diameter of 13 mm to form the sheet into a cylindrical shape. The upper end of the cylindrical sheet was clamped and hung, and less than 0.05 g of cotton (100%) was placed 300 mm below the lower end. A burner with a diameter of 10 mm was prepared and adjusted so that the gas flow rate was 105 mL / min and a blue flame 20 mm high. The burner was positioned between the cylindrical sheet and the cotton, and the bottom end of the cylindrical sheet was brought into contact with the blue flame at a position 10 mm high, and the flame was applied twice for 3 seconds. It was confirmed whether the cylindrical sheet had melted to the marked line by this operation, and whether the cotton (100%) had burned due to ignition caused by the molten sheet falling, and was evaluated according to the following criteria. A was a pass, and B and C were fail. A (good): The melting of the cylindrical sheet did not reach the marked line, and there was no combustion of the cotton. B (Poor): The melting of the cylindrical sheet reached the marked line, but the cotton did not burn. C (very poor): The melted cylindrical sheet reached the marked line, and the cotton was also burned.

[0072] (Flame retardancy: fire spread time) As in the UL94 VTM test, a flame was applied to a cylindrical sheet of flame-retardant thermoplastic resin film for 3 seconds, and the time it took for the flame to go out was measured and rated according to the following criteria: A and B are pass, and C is fail. A (Very good): The fire was extinguished in less than 15 seconds. B (Good): The fire was extinguished in 15 to 20 seconds. C (Poor): The fire was extinguished in 20 seconds or more, or was not extinguished at all.

[0073] (Coatability) The viscosity of an aqueous flame-retardant coating composition having a solid content concentration of 10% by weight was measured using a B-type viscometer at a rotor rotation speed of 60 rpm and 20°C, and the composition was evaluated according to the following criteria: A to C are acceptable, and D is unacceptable. A (very good): Viscosity is 100 to 500 mPa s B (Good): Viscosity is 50 mPa·s or more but less than 100 mPa·s, or more than 500 mPa·s but less than 1500 mPa·s C (normal): Viscosity is 5 mPa·s or more but less than 50 mPa·s, or 1500 mPa·s or more but less than 8000 mPa·s D (bad): Viscosity is less than 5 mPa·s or more than 8000 mPa·s

[0074] (Surface strength) A 5 cm long piece of cellophane tape manufactured by Nichiban Co., Ltd. was applied to the surface of the flame retardant layer, and then 2.5 cm of the tape was peeled off by hand at a low speed (2.5 cm / s) and the remaining 2.5 cm was peeled off at a high speed (25 cm / s). The surface strength was evaluated according to the degree of peeling of the flame retardant layer after peeling, and was rated according to the following criteria. 2 or more is pass, and 1 is fail. 5: No peeling at both low and high speeds. 4: No peeling at low speed, partial peeling at high speed (less than 50% of the entire high-speed peeled surface). 3: No peeling at low speed, but complete peeling (50% or more of the entire high-speed peeled surface) at high speed. 2: Peeled partially at low speed (less than 50% of the entire low-speed peeled surface), and completely at high speed (more than 50% of the entire high-speed peeled surface). 1: Peeling occurred completely at both low and high speeds.

[0075] [Table 1]

[0076] From the above results, it was confirmed that the flame-retardant layer formed by the aqueous coating composition according to the present embodiment has excellent coatability and can form a thin coating film. In addition, since it shows excellent flame retardancy, it was found that even a thin coating film can impart sufficient flame retardancy to a substrate.

[0077] Although the present invention has been described in detail and with reference to specific embodiments, it is apparent to those skilled in the art that various changes and modifications can be made without departing from the spirit and scope of the present invention. This application is based on a Japanese patent application (Patent Application No. 2020-058709) filed on March 27, 2020, the contents of which are incorporated herein by reference. [Industrial Applicability]

[0078] The water-based coating composition according to the present invention can be applied thinly and shows excellent flame retardancy even in a small amount, and is therefore very useful for imparting high flame retardancy to a substrate while forming a thin flame-retardant layer that does not impair the properties of the substrate.

Claims

1. The composition contains an inorganic phosphate, inorganic particles, a water-based binder resin that is soluble or dispersible in water, and water, the content of the aqueous binder resin is 3 to 60 parts by mass relative to 100 parts by mass of the inorganic phosphate and the inorganic particles in total, The aqueous flame-retardant coating composition, wherein the aqueous binder resin is crosslinked with at least one crosslinking agent selected from the group consisting of a metal crosslinking agent, an epoxy crosslinking agent, an epichlorohydrin crosslinking agent, and an oxazoline crosslinking agent.

2. The aqueous flame-retardant coating composition according to claim 1, wherein the mass ratio of said inorganic phosphate to said inorganic particles is 95:5 to 50:

50.

3. The aqueous flame-retardant coating composition according to claim 1 or 2, wherein the inorganic phosphate comprises ammonium polyphosphate.

4. The aqueous flame-retardant coating composition according to any one of claims 1 to 3, wherein the inorganic particles contain a layered silicate.

5. the aqueous binder resin contains an acrylic resin, The aqueous flame-retardant coating composition according to any one of claims 1 to 4, wherein the acrylic resin is dispersed in the aqueous flame-retardant coating composition.

6. A flame-retardant thermoplastic resin film, comprising a layer formed on at least one surface of the thermoplastic resin film from the aqueous flame-retardant coating composition according to any one of claims 1 to 5.

7. A flame-retardant layer is provided on at least one surface of a thermoplastic resin film, the flame-retardant layer containing an inorganic phosphate, inorganic particles, and an aqueous binder resin that is soluble or dispersible in water; the content of the aqueous binder resin is 3 to 60 parts by mass relative to 100 parts by mass of the inorganic phosphate and the inorganic particles in total, The flame-retardant thermoplastic resin film, wherein the aqueous binder resin is crosslinked with at least one crosslinking agent selected from the group consisting of a metal-based crosslinking agent, an epoxy-based crosslinking agent, an epichlorohydrin-based crosslinking agent, and an oxazoline-based crosslinking agent.

8. The flame-retardant thermoplastic resin film according to claim 7, wherein the mass ratio of the inorganic phosphate to the inorganic particles is 95:5 to 50:

50.

9. The resin component of the thermoplastic resin film is 100 g / m 2 whereas the inorganic phosphate in the flame retardant layer is 1 to 45 g / m 2 and the inorganic particles are 0.1 to 25 g / m 2 The flame-retardant thermoplastic resin film according to claim 7 or 8,

10. The resin component of the thermoplastic resin film is 100 g / m 2 whereas the total amount of the inorganic phosphate and the inorganic particles in the flame-retardant layer is 50 g / m 2 The flame-retardant thermoplastic resin film according to any one of claims 7 to 9, wherein the flame-retardant thermoplastic resin film has a flame retardant viscosity of less than 100°C.

11. The flame-retardant thermoplastic resin film according to any one of claims 7 to 10, further comprising at least one of a printing layer and a print-receiving layer on a surface of the flame-retardant layer opposite to the side on which the thermoplastic resin film is located.

Citation Information

Patent Citations

  • Finishing method of flame-retardant and heat-resistant linen fabric

    CN105463853A

  • Fire retarding resin composition

    JP2003171569A

  • Coating composition for interior material of car and interior material for car

    JP2006176729A

  • Coating composition and motor vehicle interior trim material

    JP2007186686A

  • Combustion-stopping composition and combustion-stopping prepreg and incombustible decorative laminated sheet

    JP2007246697A