Solid-state imaging device and its manufacturing method
The solid-state image sensor's outer peripheral film with a protruding, uneven shape addresses the issue of antireflection film peeling, enhancing manufacturing efficiency and reducing costs by maintaining film integrity.
Patent Information
- Application Number
- JP2022548115
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-12-10
- Filing Date
- 2021-12-10
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2041-12-10
AI Technical Summary
Conventional methods for forming an antireflection film on solid-state image sensors result in cracking or peeling at the outer edge due to the use of resin materials with higher thermal expansion, leading to manufacturing inefficiencies and increased costs.
A solid-state image sensor design with an outer peripheral film having a protruding, uneven shape that follows the lens shape, featuring a resin layer with convex portions that enhance the bending strength of the antireflection film, preventing peeling during manufacturing processes.
The design effectively prevents antireflection film peeling, ensuring efficient manufacturing and reducing manufacturing time and costs by maintaining film integrity during cleaning and other processes.
Smart Images

Figure 0007594017000002 
Figure 0007594017000003 
Figure 0007594017000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a solid-state imaging device and a manufacturing method thereof. This application claims priority to Japanese Patent Application No. 2020-204965, filed in Japan on December 10, 2020, the contents of which are incorporated herein by reference. [Background technology]
[0002] The solid-state imaging element has a plurality of photoelectric conversion elements, filters, and lenses stacked in this order on a substrate. Each photoelectric conversion element, filter, and lens forms an imaging pixel, and is arranged in the center of the solid-state imaging element. To improve imaging sensitivity, an anti-reflection film is often formed on the surface of each lens. The anti-reflection film is a thin film made of an inorganic material such as silicon dioxide, and is prone to cracking when formed on a lens made of a resin material with a larger thermal expansion coefficient. Patent document 1 proposes a technology in which, in a solid-state imaging element, multiple convex bodies are provided in the peripheral region adjacent to the effective light-receiving area, the convex bodies being made of the same material as the microlenses so as to surround the effective light-receiving area, and an anti-reflection coating is formed that uniformly covers the surfaces of the microlenses and the convex bodies. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Japanese Patent Publication No. 2013-12518 Summary of the Invention [Problem to be solved by the invention]
[0004] However, the above-mentioned conventional techniques have the following problems. The technology described in Patent Document 1 is a technology for preventing cracks from occurring in an anti-reflection film on a microlens at the outer edge of an effective light-receiving area. However, the solid-state imaging device has a peripheral region that does not have photoelectric conversion elements and extends beyond the peripheral region. Since wiring connected to the photoelectric conversion elements is formed on the substrate in the peripheral region, a flat light-shielding layer is formed on the substrate in the peripheral region to prevent reflection of light incident from the outside. A resin layer made of the same material as the microlenses is laminated on top of the light-shielding layer, and the anti-reflection film also covers this resin layer. In order to expose the scribe and electrode pads of the solid-state imaging element, a part of the resin layer in the peripheral region is removed by etching after the anti-reflection film is formed, thereby adjusting the shape of the outer edge of the peripheral region. In this etching process, the side surface of the resin layer is eroded, so that after etching, a part of the anti-reflection film is left in a state where the outer edge of the resin layer protrudes. The protruding anti-reflection film may crack or peel off in a subsequent process such as a cleaning process, which may cause defects in the solid-state imaging device. In order to prevent such damage to the anti-reflective coating, it is also possible to carry out the etching process after forming a resin coating layer around the outer edge of the anti-reflective coating. In this case, the erosion of the resin layer that accompanies the progress of etching occurs below the outer coating layer of the anti-reflective coating, so that the erosion of the resin layer below the anti-reflective coating can be prevented. However, this manufacturing method requires a step of forming a coating layer, which increases the manufacturing time and costs.
[0005] The present invention has been made in view of the above problems, and has an object to provide a solid-state imaging device capable of preventing peeling of the antireflection film at the outer edge. It is yet another object of the present invention to provide a method for efficiently manufacturing a solid-state imaging device that can prevent peeling of the outer edge of the antireflection film. [Means for solving the problem]
[0006] In order to solve the above problems, a solid-state imaging device according to a first aspect of the present invention includes a substrate, a plurality of photoelectric conversion elements arranged on the substrate, a filter section arranged above the plurality of photoelectric conversion elements and transmitting light incident on the plurality of photoelectric conversion elements, a plurality of lenses arranged above the filter section, and Multiple Lenses a resin layer arranged so as to surround from the outside an outer edge of the lenses in a plan view, and an anti-reflection film formed on the plurality of lenses and the resin layer, the anti-reflection film having an outer peripheral film covering an outer peripheral portion of the resin layer in a plan view, the outer peripheral portion of the resin layer having a lens shape, On the substrate, there are provided an effective light-receiving area (A1), a peripheral light-shielding area (A2) adjacent to an outer edge of the effective light-receiving area (A1), and a substrate outer periphery area (A3) which is an area from the outer edge of the peripheral light-shielding area (A2) to the outer edge of the substrate, The outer peripheral film has an uneven shape having unevenness following the lens shape in a thickness direction of the resin layer, and at least a part of an outer edge of the outer peripheral film protrudes outward beyond the resin layer. The protrusion has a protruding portion in the substrate outer peripheral region (A3), Curved in the thickness direction following the lens shape In the substrate outer peripheral region (A3), an electrode pad is formed on the substrate, and the protrusion is provided to protrude from the outer edge of the peripheral light-shielding region (A2) in a region of the substrate outer peripheral region (A3) where the electrode pad is not provided, in a plan view of the resin layer. .
[0010] In the above solid-state imaging element, a light-shielding layer that absorbs external light may be further provided between the substrate and the resin layer, the filter portion may have a plurality of colored layers, and at least a portion of the light-shielding layer may be formed by the colored layers.
[0011] In the solid-state imaging device, a maximum amount of protrusion of the outer peripheral film from the resin layer may be 40% or more and 200% or less of a pixel size determined by an arrangement pitch of the plurality of photoelectric conversion elements.
[0012] In the solid-state imaging device, the uneven shape of the outer peripheral film may have two or more convex portions in a direction from an outer edge of the resin layer toward an inside thereof.
[0013] In the solid-state imaging device, the uneven shape of the outer peripheral film may be such that an arrangement pitch of convex portions of the uneven shape is equal to an arrangement pitch of the plurality of lenses.
[0014] In the above solid-state imaging element, the anti-reflection film may have an internal film formed on the plurality of lenses and an intermediate film disposed between the internal film and the outer peripheral film, and the intermediate film may be formed flat.
[0015] A method for manufacturing a solid-state imaging device according to a second aspect of the present invention includes preparing a substrate on which a plurality of photoelectric conversion elements are formed, forming a filter portion above the plurality of photoelectric conversion elements to cover the plurality of photoelectric conversion elements, and On the filter forming a resin layer on the filter portion; patterning the resin layer to form a plurality of lenses covering the plurality of photoelectric conversion elements on the filter portion, and a lens shape having unevenness in a thickness direction on an outer periphery of the resin layer in a plan view, on the resin layer; forming an anti-reflection film on a surface of the patterned resin layer; and etching an outer periphery of the anti-reflection film and an outer periphery of the resin layer over an entire periphery so that at least a part of an outer periphery of the anti-reflection film protrudes from the resin layer and is curved following the lens shape in the thickness direction, thereby removing a part of the anti-reflection film and the resin layer. On the substrate, there are provided an effective light-receiving region (A1), a peripheral light-shielding region (A2) adjacent to the outer edge of the effective light-receiving region (A1), and a substrate outer periphery region (A3) which is a region from the outer edge of the peripheral light-shielding region (A2) to the outer edge of the substrate, and in the substrate outer periphery region (A3), an electrode pad is formed on the substrate, and at least a part of the outer edge of the anti-reflection film protrudes from the outer edge of the peripheral light-shielding region (A2) into a region of the substrate outer periphery region (A3) where the electrode pad is not provided, in a plan view of the resin layer. . Effect of the Invention
[0016] According to the solid-state imaging device of the present invention, peeling of the antireflection film at the outer edge can be prevented. According to the method for manufacturing a solid-state imaging device of the present invention, it is possible to efficiently manufacture a solid-state imaging device capable of preventing peeling of the outer edge of the antireflection film. [Brief description of the drawings]
[0017] [Figure 1] 1 is a schematic plan view illustrating an example of a solid-state imaging element according to an embodiment of the present invention. [Diagram 2] FIG. 2 is an enlarged view of part F2 in FIG. [Diagram 3] FIG. 3 is a cross-sectional view taken along line F3-F3 in FIG. [Figure 4] FIG. 3 is a cross-sectional view taken along line F4-F4 in FIG. [Diagram 5] FIG. 2 is an enlarged view of part F5 in FIG. [Figure 6] FIG. 6 is a cross-sectional view taken along line F6-F6 in FIG. [Figure 7] FIG. 7 is a side view taken along the line F7 in FIG. [Figure 8] 5A to 5C are schematic diagrams illustrating an example of a method for manufacturing a solid-state imaging device according to an embodiment of the present invention. [Figure 9] 5A to 5C are schematic diagrams illustrating an example of a method for manufacturing a solid-state imaging device according to an embodiment of the present invention. [Figure 10] 5A to 5C are schematic diagrams illustrating an example of a method for manufacturing a solid-state imaging device according to an embodiment of the present invention. [Figure 11] 5A to 5C are schematic diagrams illustrating an example of a method for manufacturing a solid-state imaging device according to an embodiment of the present invention. [Figure 12] 5A to 5C are schematic diagrams illustrating an example of a method for manufacturing a solid-state imaging device according to an embodiment of the present invention. [Figure 13] 5A to 5C are schematic diagrams illustrating an example of a method for manufacturing a solid-state imaging device according to an embodiment of the present invention. [Figure 14] 5A to 5C are schematic diagrams illustrating an example of a method for manufacturing a solid-state imaging device according to an embodiment of the present invention. [Figure 15] 5A to 5C are schematic diagrams illustrating a method for manufacturing a solid-state imaging device according to a comparative example. [Figure 16] 5A to 5C are schematic diagrams illustrating a method for manufacturing a solid-state imaging device according to a comparative example. [Figure 17] 10A to 10C are cross-sectional views showing examples of damage forms of a solid-state imaging element of a comparative example. [Figure 18] 10A to 10C are cross-sectional views showing examples of damage forms of a solid-state imaging element of a comparative example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] A solid-state imaging device and a manufacturing method thereof according to an embodiment of the present invention will be described below. FIG. 1 is a schematic plan view showing an example of a solid-state imaging device according to an embodiment of the present invention.
[0019] As shown in FIG. 1, a plurality of solid-state imaging elements 1 of this embodiment are formed on a silicon wafer W by a semiconductor manufacturing process. The outer shape of each solid-state imaging element 1 in a plan view is a rectangle surrounded by scribes S formed in a rectangular lattice pattern. Each solid-state imaging element 1 is cut and separated along the scribes S, and then mounted in a package. In the following, the silicon wafer W cut and separated along the scribes S is referred to as a semiconductor substrate 2. However, in explaining the manufacturing method, when explaining an example of each solid-state imaging element 1, the silicon wafer W may be simply referred to as a semiconductor substrate 2. The semiconductor substrate 2 has a rectangular outer shape in a plan view. Here, "plan view" means that the semiconductor substrate 2 is viewed in the thickness direction. There is no particular limitation on the type of the solid-state imaging device 1 as long as it is an area sensor capable of capturing a color image. For example, the solid-state imaging device 1 may be of a CCD type or a CMOS type.
[0020] The solid-state imaging device 1 has, on a semiconductor substrate 2, an effective light-receiving area A1, a peripheral light-shielded area A2, and a substrate peripheral area A3. The effective light-receiving area A1 is a rectangular area in a plan view in which imaging pixels are arranged. The effective light-receiving area A1 is formed in the center of the semiconductor substrate 2. The peripheral light-shielding region A2 is a rectangular frame-shaped region adjacent to the outer edge of the effective light-receiving region A1 and surrounding the entire outer edge from the outside. The peripheral light-shielding region A2 includes a layer portion that blocks incident light from outside and its reflected light. The peripheral light-shielding region A2 is made up of an inner peripheral portion A2a adjacent to the effective light-receiving region A1 and an outer peripheral portion A2b that includes the outer edge of the peripheral light-shielding region A2. The substrate peripheral region A3 is a region from the outer edge of the peripheral light-shielding region A2 to the outer edge of the semiconductor substrate 2. A plurality of metal electrode pads 9 for wiring the solid-state imaging element 1 are formed on the semiconductor substrate 2 in the substrate peripheral region A3.
[0021] The cross-sectional configurations of the effective light-receiving area A1 and the inner periphery A2a of the peripheral light-shielded area A2 will be described. Fig. 2 is an enlarged view of a portion F2 in Fig. 1. Fig. 3 is a cross-sectional view taken along line F3-F3 in Fig. 2. Fig. 4 is a cross-sectional view taken along line F4-F4 in Fig. 2.
[0022] As shown in FIG. 2, lenses 7 for collecting external light are formed in the effective light receiving area A1 in correspondence with each imaging pixel. In the peripheral light-shielded area A2 adjacent to the effective light-receiving area A1, an inner convex body 17 having the same shape as the lens 7 is formed adjacent to the lens 7. In the peripheral light-shielding region A2, a flat resin layer 27 is adjacent to the outer periphery side (the right side in the figure) of the inner convex body 17. The inner periphery A2a of the peripheral light-shielding region A2 is a region in which the inner convex body 17 and the flat resin layer 27 are formed in a plan view.
[0023] As shown in FIG. 3, in the effective light-receiving area A1, a photoelectric conversion element 3, a first planarization layer 4, a filter portion 5, a second planarization layer 6, a lens 7 and an anti-reflection film 8 are formed on a semiconductor substrate 2 in this order. The photoelectric conversion element 3 converts incident light into an electric signal and outputs an electric signal according to the amount of received light. In this embodiment, a large number of the photoelectric conversion elements 3 are arranged in a rectangular lattice shape along the vertical and horizontal directions of the effective light-receiving area A1, which is rectangular in plan view.
[0024] The first planarization layer 4 is a transparent resin layer laminated on the semiconductor substrate 2 and the photoelectric conversion element 3. The first planarization layer 4 smoothes out irregularities formed on the surfaces of the semiconductor substrate 2 and the photoelectric conversion element 3, and forms a flat surface above the semiconductor substrate 2 and the photoelectric conversion element 3. The first planarization layer 4 is formed, for example, by spin-coating a colorless and transparent acrylic resin solution to a thickness of about 0.1 μm and curing it by heat treatment.
[0025] The filter section 5 is a layer section that separates the color of incident light from the outside of the solid-state imaging device 1 , and is laminated on the first planarization layer 4 . For example, the filter section 5 has a red colored layer 5r having a spectral characteristic of transmitting red light, a green colored layer 5g having a spectral characteristic of transmitting green light, and a blue colored layer 5b having a spectral characteristic of transmitting blue light. Each colored layer in the filter section 5 is disposed facing a photoelectric conversion element 3 in a one-to-one relationship in the thickness direction of the solid-state imaging device 1. Each colored layer does not necessarily have to be disposed facing a photoelectric conversion element 3 in a one-to-one relationship. For example, one colored layer may be disposed corresponding to four photoelectric conversion elements. Any known suitable arrangement can be adopted as the arrangement of the colored layers of the filter section 5. In the following, an example in which the colored layers are arranged based on the Bayer arrangement will be described. In the Bayer array, a red colored layer 5r and a blue colored layer 5b are arranged in a diagonal direction in a 2×2 rectangular array, and two green colored layers 5g are arranged in the opposite diagonal direction. Therefore, in the cross section shown in Fig. 3, the green colored layers 5g and the blue colored layers 5b are alternately arranged adjacent to each other in the horizontal direction in the figure. In the adjacent row of the filter portion 5 in this cross section, the green colored layers 5g and the red colored layers 5r are alternately arranged adjacent to each other in the horizontal direction in the figure as shown in Fig. 4. The filter portion 5 is disposed up to the region where the inner convex body 17 is formed in the thickness direction. However, the red colored layer 5r, the green colored layer 5g, and the blue colored layer 5b do not have to be directly adjacent to each other as in the examples shown in Figures 3 and 4. For example, a lattice-shaped partition wall may be formed on the first planarization layer 4, and any one of the red colored layer 5r, the green colored layer 5g, and the blue colored layer 5b may be embedded on the first planarization layer 4 inside the partition wall to form the filter portion 5.
[0026] The filter section 5 can be formed by forming a red colored layer 5r, a green colored layer 5g, and a blue colored layer 5b on the first planarization layer 4. A specific colored layer can be formed by spin-coating a coloring material such as a pigment having the spectral transmittance characteristics and a photosensitive material containing an alkali-soluble resin on the first planarization layer 4, patterning the photosensitive material by a photolithography method including exposure and development steps, and curing the photosensitive material. The order of forming the red colored layer 5r, the green colored layer 5g, and the blue colored layer 5b is not particularly limited.
[0027] Since the thickness required to obtain the required spectral transmittance is likely to differ depending on the colored layer, the filter portion 5 is likely to have fine irregularities on its surface even if the first planarizing layer 4 is flat. 3 and 4, in this embodiment, a second planarization layer 6 for planarizing the irregularities on the surface of the filter portion 5 is laminated on the filter portion 5. The second planarization layer 6 is a transparent resin layer. The material of the second planarizing layer 6 is not particularly limited as long as it is a transparent resin material that can form a flat surface.
[0028] The lenses 7 focus light incident on the solid-state imaging device 1 from the outside onto each photoelectric conversion element 3. The lenses 7 are formed on the second planarization layer 6 at a position facing the photoelectric conversion element 3 with the red colored layer 5r, the green colored layer 5g, or the blue colored layer 5b sandwiched therebetween. For this reason, the lenses 7 are arranged in a rectangular lattice shape that matches the arrangement pitch of the photoelectric conversion elements 3 arranged in the vertical and horizontal directions. The arrangement pitch may be different in the vertical and horizontal directions, but in this embodiment, the size of the arrangement pitch in both the vertical and horizontal directions is P. The size of the arrangement pitch P is determined by the pixel density of the solid-state imaging device 1 and is not particularly limited. The shape of lens 7 is not particularly limited as long as it is a convex lens shape that can efficiently collect external light onto photoelectric conversion element 3 . There is no particular limitation on the material of the lens 7 as long as it is a transparent resin material, for example, acrylic, novolac, etc. The material of the lens 7 may be different from that of the second planarization layer 6, or may be the same as that of the second planarization layer 6.
[0029] For example, there is no particular limitation on the manufacturing method of the lens 7. For example, the lens 7 may be manufactured using a reflow type or transfer type manufacturing method. In the reflow type manufacturing method, an acrylic photosensitive resin, which is the material of the lens 7, is selectively patterned by photolithography, and then the lens shape is formed by utilizing the thermal reflow property of the material. In the transfer type manufacturing method, a lens master is formed on a flat layer of transparent acrylic resin, which is the material for lens 7, by photolithography and thermal reflow using a resist material that is alkali-soluble, photosensitive, and thermally reflowable, and the shape of the lens master is transferred to the transparent acrylic resin layer by dry etching.
[0030] The anti-reflection film 8 is a thin film that suppresses reflection on the surface of the lens 7. The anti-reflection film 8 is uniformly formed on the convex surface of the lens 7. The surface of the anti-reflection film 8 has an uneven shape that follows the uneven shape formed by the multiple lenses 7. The lens 7, the inner convex body 17, the flat resin layer 27, and the second flattening layer 6 may be made of the same material. In this case, there is no boundary between the lens 7, the inner convex body 17, the flat resin layer 27, and the second flattening layer 6, and they are formed integrally. In this configuration, the anti-reflection film 8 is formed on the lens 7, the inner convex body 17, and the flat resin layer 27, which are made of the same material as the second flattening layer 6. The antireflection film 8 may be a multilayer film or a single layer film. When the antireflection film 8 is a multilayer film, it may be a multilayer antireflection film having two or more layers in which high refractive index layers and low refractive index layers are alternately laminated. Examples of materials for the high refractive index layer used in the multilayer antireflection coating include oxides of metals such as titanium, cerium, tantalum, tin, indium, zirconium, and aluminum, or mixtures of these metal oxides. The refractive index of the high refractive index layer may be, for example, 1.60 or more. The material of the low refractive index layer used in the multilayer antireflection film may be an oxide of a metal such as magnesium, zirconium, or aluminum, a silicon-based oxide such as silicon dioxide, magnesium fluoride, or a mixture of these compounds. The refractive index of the low refractive index layer is not particularly limited as long as it is lower than that of the high refractive index layer. For example, the refractive index of the low refractive index layer may be less than 1.60.
[0031] When the antireflection film 8 is formed as a single layer film, a material having a refractive index lower than that of the material of the lens 7 is used as the material of the antireflection film 8. For example, the above-mentioned low refractive index layer may be used as the material of the single layer film. For example, by forming a film of silicon dioxide with a refractive index of 1.46 on the surface of the lens 7 to a thickness of 50 nm to 200 nm, a single-layer anti-reflection film 8 capable of suppressing the reflectance of visible light can be formed.
[0032] The anti-reflection film 8 can be formed by depositing the above-mentioned inorganic material using a vacuum film-forming technique such as vacuum deposition or sputtering. Of the thin film materials that can be used for the anti-reflection coating 8, it is particularly preferable to include silicon dioxide as a constituent material of the anti-reflection coating 8, since this allows for easy formation of low-cost, high-quality thin films using vacuum deposition techniques, and the optical properties and durability of thin films are well known.
[0033] In the inner periphery A2a of the peripheral light-shielding region A2, a first planarization layer 4, an inner light-shielding layer 15, and a second planarization layer 6 are formed in this order on the semiconductor substrate 2. An inner convex body 17 and a flat resin layer 27 are formed on the second planarization layer 6 in the inner periphery A2a, and an anti-reflection film 8 similar to that in the effective light-receiving region A1 is formed on the surfaces of the inner convex body 17 and the flat resin layer 27. However, the surface shape of the anti-reflection film 8 in the inner periphery A2a follows the surface shapes of the inner convex body 17 and the flat resin layer 27.
[0034] The first planarization layer 4 is the same layer portion as the first planarization layer 4 in the effective light-receiving region A1, and is continuous with the first planarization layer 4 in the effective light-receiving region A1.
[0035] The inner light-shielding layer 15 is provided to suppress incident light from the outside (hereinafter, external incident light) and reflected light of the incident light at the semiconductor substrate 2 (hereinafter, internal reflected light). As shown in Fig. 1, an outer peripheral surface 15a in a plan view of the inner light-shielding layer 15 extends close to an outer peripheral surface 25a of an outer light-shielding layer (light-shielding layer) 25 described below, which is the outer edge of the peripheral light-shielding region A2. The outer peripheral surface 15a in a plan view is substantially rectangular with rounded corners, similar to the outer peripheral surface 25a in a plan view. The inner light-shielding layer 15 is not particularly limited as long as it is configured to absorb at least a part of the external incident light and the internally reflected light. The inner light-shielding layer 15 may be formed as a single layer or as a multilayer. For example, the inner light-shielding layer 15 may be a colored layer colored with a coloring material of an appropriate color. For example, the inner light-shielding layer 15 may be a colored layer colored black with a black coloring material. In the example shown in FIG. 3, the red colored layer 5r and the blue colored layer 5b in the filter portion 5 are laminated in this order on the first flattening layer 4. However, the lamination order is not limited to this, and the blue colored layer 5b and the red colored layer 5r in the filter portion 5 may be laminated in this order on the first flattening layer 4. In this case, the inner light-shielding layer 15 can be formed in each manufacturing process of the blue colored layer 5b and the red colored layer 5r in the filter portion 5, so that the manufacturing process can be simplified. Similarly, the inner light-shielding layer 15 may be composed of a combination of two or more colored layers selected from the red colored layer 5r, the green colored layer 5g, and the blue colored layer 5b. However, it is more preferable to laminate the red colored layer 5r and the blue colored layer 5b, since their transmission wavelength ranges are far from each other and therefore dark colors can be easily obtained.
[0036] The second planarization layer 6 in the inner periphery A2a is the same layer portion as the second planarization layer 6 in the effective light-receiving area A1, and is continuous with the second planarization layer 6 in the effective light-receiving area A1. The second planarization layer 6 in the inner periphery A2a is formed in the same process as the second planarization layer 6 in the effective light-receiving area A1, after the filter portion 5 and the inner light-shielding layer 15 are formed.
[0037] The inner convex body 17 has the same shape as the lens 7, except that it is provided adjacent to the lens 7 in the peripheral light-shielding region A2. The inner convex body 17 is made of the same material as the lens 7 and is formed in the same manner as the lens 7. The inner convex body 17 is provided for the purpose of suppressing the occurrence of cracks in the lens 7 disposed on the outer edge of the effective light-receiving area A1. If the anti-reflection coating 8 is formed after molding of the lens 7, the stress inherent in the anti-reflection coating 8 during deposition is released, which tends to cause cracks in the anti-reflection coating 8 at the outer edge of the effective light-receiving area A1. By providing an inner convex body 17 having the same shape as the lens 7 adjacent to the outer edge of the effective light-receiving area A1, even if cracks do occur, they will remain in the area where the inner convex body 17 is formed, thereby suppressing defects in the anti-reflection coating 8 on the lens 7. Since the inner convex body 17 does not have optical properties such as a light collecting effect, even if a crack occurs in the anti-reflection film 8, the performance of the solid-state imaging element 1 does not deteriorate.
[0038] The number of inner convex bodies 17 in the direction from the effective light-receiving area A1 toward the outside is not particularly limited as long as it can suppress the intrusion of cracks into the effective light-receiving area A1. Although an example in which the inner convex bodies 17 are provided in one row surrounding the effective light-receiving area A1 is shown in Figures 3 and 4, the inner convex bodies 17 and the colored layer 5 may be provided in two or more rows.
[0039] The flat resin layer 27 is a flat layer portion provided so as to surround the inner convex body 17 from the side opposite to the effective light-receiving area A1. The flat resin layer 27 is formed of the same material as the lenses 7 and the inner convex body 17. The thickness of the flat resin layer 27 is not particularly limited, but may be the same as the thickness after curing of the layer portion applied onto the second planarizing layer 6 to form the lenses 7 and the inner convex body 17.
[0040] The configuration of the outer periphery A2b of the peripheral light-shielded area A2 will be described. Fig. 5 is an enlarged view of a portion F5 in Fig. 1. Fig. 6 is a cross-sectional view taken along line F6-F6 in Fig. 5. Fig. 7 is a side view taken along line F7 in Fig. 6.
[0041] As shown in FIG. 5, the outer circumferential portion A2b is formed adjacent to the outer edge of the inner circumferential portion A2a. In the outer peripheral portion A2b in the cross section shown in Figure 6, a first planarization layer 4, an outer light-shielding layer 25, a second planarization layer 6, an outer convex body 37 (convex portion, resin layer), and an anti-reflection film 8 are formed in this order on the semiconductor substrate 2. However, as shown in FIG. 6, an inner light-shielding layer 15 is formed on a part of the inner periphery A2a.
[0042] As shown in FIG. 6, the first planarization layer 4 is the same layer portion as the first planarization layer 4 in the effective light-receiving area A1 and the inner periphery A2a, and is continuous with the first planarization layer 4 in the inner periphery A2a. The outer light-shielding layer 25 is a layer portion adjacent to the outer peripheral surface 15a of the inner light-shielding layer 15 and surrounding the outside of the inner light-shielding layer 15. As shown in Fig. 1, the outer peripheral surface 25a of the outer light-shielding layer 25 forms the outer edge of the peripheral light-shielding region A2. In addition, in the thickness direction of the solid-state imaging element 1, the outer light-shielding layer 25 is preferably formed between the outer convex body 37 and the semiconductor substrate 2. The outer light-shielding layer 25 is provided to suppress external incident light and internal reflected light, similar to the inner light-shielding layer 15. As shown in Fig. 1, an outer peripheral surface 25a in a plan view has a substantially rectangular shape with rounded corners. The outer light-shielding layer 25 is formed outside the inner light-shielding layer 15 in a plan view and is formed farther from the effective light-receiving area A1, so that its light-shielding performance may be lower than that of the inner light-shielding layer 15 closer to the peripheral light-shielding area A2. The outer light-shielding layer 25 is not particularly limited as long as it is configured to absorb at least a part of the external incident light and the internally reflected light. The outer light-shielding layer 25 may be formed of a single layer film or a multilayer film. For example, the outer light-shielding layer 25 may be a colored layer colored with a coloring material of an appropriate color. For example, when the outer light-shielding layer 25 is formed of a single layer film, the outer light-shielding layer 25 may be formed of the same material as any one of the red colored layer 5r, the green colored layer 5g, and the blue colored layer 5b. Particularly preferred is the blue colored layer 5b or the red colored layer 5r. In this embodiment, the blue colored layer 5b of the filter portion 5 is laminated on the first planarization layer 4 to the same thickness as the inner light-shielding layer 15. In this case, the outer light-shielding layer 25 can be formed in the manufacturing process of the blue colored layer 5b of the filter portion 5, thereby simplifying the manufacturing process.
[0043] The second planarization layer 6 in the outer circumferential portion A2b is the same layer portion as the second planarization layer 6 in the effective light-receiving area A1 and the inner circumferential portion A2a, and is continuous with the second planarization layer 6 in the inner circumferential portion A2a. The second planarization layer 6 in the outer periphery A2b is formed in the same process as the second planarization layer 6 in the effective light-receiving area A1, after the inner light-shielding layer 15 and the outer light-shielding layer 25 are formed.
[0044] The outer convex body 37 is provided on the outer peripheral portion A2b as shown in FIG. 5. The outer convex body 37 is a layered portion that forms an uneven shape having unevenness in the thickness direction of the outer light-shielding layer 25 on the antireflection film 8 in the outer peripheral portion A2b as shown in FIG. 6. The surface shape of the outer convex body 37 is not particularly limited as long as it can form an uneven shape that improves the bending strength of the antireflection film 8. A particularly preferred uneven shape is a waveform in which concaves and convexities appear alternately in the thickness direction of the outer light-shielding layer 25 when the antireflection film 8 is viewed from the outer edge side to the inside. The shape of the waveform may be sinusoidal or a waveform other than a sinusoidal wave, for example, a waveform with continuous upwardly convex arcs. The larger the amplitude of the waveform, the larger the moment of area becomes, so it is more preferable.
[0045] In this embodiment, the outer convex body 37 has the same shape as the lens 7, except that it is provided on the outer circumferential portion A2b. Furthermore, the outer convex bodies 37 are arranged in the same rectangular lattice pattern as the lenses 7, with the same arrangement pitch P as the lenses 7. Therefore, in this embodiment, when the effective light-receiving area A1 is located on an extension line of the row of the outer convex bodies 37 extending in the vertical or horizontal direction, the row of the outer convex bodies 37 is located in the same row as the row of the lenses 7 in the effective light-receiving area A1. The outer convex body 37 is formed in the same manner as the lens 7 and from the same material as the lens 7. In this case, the outer convex body 37 can be manufactured at the same time as the lens 7, and therefore the manufacturing process can be simplified.
[0046] As shown in FIG. 5, a plurality of outer convex bodies 37 are arranged from the inside or outside of outer circumferential surface 15a toward outer circumferential surface 25a. As shown in FIG. 6, the outer periphery of the second planarizing layer 6 and the outer convex body 37 is broken in the thickness direction, and an outer periphery E intersecting with the surface of the semiconductor substrate 2 is formed as the broken surface. Since FIG. 6 is a schematic diagram, the outer peripheral surface E is depicted as standing perpendicular to the surface of the semiconductor substrate 2; however, as described below, the outer peripheral surface E is formed by etching, and therefore the outer peripheral surface E may be inclined from the vertical or curved with respect to the vertical plane.
[0047] As shown in FIG. 1, the outer circumferential surface E in plan view runs along the outer circumferential surface 25a and on the inside of the outer circumferential surface 25a. Three or more outer convex bodies 37 are lined up, excluding the outer convex bodies 37 broken by the outer peripheral surface E. Note that, in this embodiment, three or more outer convex bodies 37 are lined up, but from the viewpoint of preventing peeling, it is sufficient that two or more are lined up. In particular, in the area where the outer peripheral surface E is curved, the outer convex body 37 is disposed outside the outer peripheral surface 15a and inside the outer peripheral surface 25a, as shown in Fig. 5. Therefore, the outer convex body 37 is disposed in a band shape along the outer peripheral surface E. The surface of the group of outer convex bodies 37 forms an uneven shape in which upwardly convex lens surface shapes are arranged two-dimensionally.
[0048] As shown in Figure 6, the anti-reflection coating 8 in the outer peripheral portion A2b is similar to the anti-reflection coating 8 on the lens 7, except that it is formed on the surface of the outer convex body 37 and at least a portion of the anti-reflection coating 8 formed on the outer convex body 37 that intersects with the outer peripheral surface E protrudes outward beyond the outer peripheral surface E. As described above, the anti-reflection film 8 in this embodiment includes a first anti-reflection film 8a (see Figures 3 and 4) formed on the lens 7, a second anti-reflection film 8b (see Figures 3 and 4) formed on the inner convex body 17, a third anti-reflection film 8c (see Figures 3, 4 and 6) formed on the flat resin layer 27, and a fourth anti-reflection film 8d (see Figure 6) formed on the outer convex body 37. Since all of the anti-reflection coatings 8 are formed in the same process described below, they have the same film thickness, and since the inner convex body 17, the flat resin layer 27, and the outer convex body 37 are all made of the same material as the lens 7, they each have the same anti-reflection function.
[0049] The first antireflection film 8a is an internal film formed on each lens 7 in the effective light-receiving area A1. The first antireflection film 8a is formed in a rectangular region in the center of the antireflection film 8 in a plan view. In contrast, the fourth antireflection film 8d is formed on the outer periphery of the antireflection film 8 in a planar view, and is an outer peripheral film that covers the area in which the outer light-shielding layer 25 or the inner light-shielding layer 15 is formed. The third antireflection film 8c is a flat intermediate film between the first antireflection film 8a, which is the internal film, and the fourth antireflection film 8d, which is the peripheral film, covering part of the area where the inner light-shielding layer 15 is formed or part of the area where the outer light-shielding layer 25 is formed.
[0050] The fourth antireflection film 8d has a protruding portion 8e that protrudes outward from the outer circumferential surface E in at least a part of the outer edge in a plan view. As described below, the protrusion 8e in the fourth anti-reflection film 8d is formed when the etching gas erodes the side surface of the outer convex body 37 when the outer convex body 37 outside the outer edge of the fourth anti-reflection film 8d is etched and removed after the fourth anti-reflection film 8d is formed on the outer convex body 37. Here, when the outer peripheral surface E is inclined or curved in the height direction, the protrusion amount d is the value measured from the point e where the outer peripheral surface E of the outer convex body 37 contacts the fourth antireflection film 8d in a plan view. In this embodiment, the fourth anti-reflection film 8d has an uneven shape in the thickness direction of the outer light-shielding layer 25, both in the cross section in the protruding direction as shown in FIG. 6 and when viewed from the protruding direction as shown in FIG. 7. This improves the bending strength and bending rigidity of the fourth anti-reflection film 8d. Therefore, the maximum value of the protruding amount d is 40% or more and 200% or less of the arrangement pitch P of the outer convex bodies 37. This configuration makes it possible to prevent the fourth anti-reflection film 8d from peeling off due to external forces such as water pressure in a cleaning process. In addition, if the maximum value of the protruding amount d exceeds 100% of the arrangement pitch P of the outer convex bodies 37, the rate at which the protruding portion 8e is chipped increases, so from the viewpoint of chipping prevention, the maximum value of the protruding amount d is preferably 40% or more and 100% or less of the arrangement pitch P of the outer convex bodies 37, and more preferably 40% or more and 70% or less.
[0051] Table 1 shows the evaluation of the solid-state imaging device in this embodiment. The pixel size and the maximum protrusion amount were changed in the semiconductor imaging elements of Examples 1 to 6. In Examples 1 and 2, the pixel size (arrangement pitch P) was 1.1 μm, and in Examples 3 to 6, the pixel size (arrangement pitch P) was 1.0 μm. Note that the pixel size shown in these examples is just an example. The maximum value of the protrusion amount d was 0.46 μm in Example 1, 0.51 μm in Example 2, 0.63 μm in Example 3, 0.80 μm in Example 4, 0.92 μm in Example 5, and 1.04 μm in Example 6. As a result, the ratio of the maximum value of the protrusion amount d to the arrangement pitch P of the outer convex bodies 37 was 42% in Example 1, 46% in Example 2, 63% in Example 3, 80% in Example 4, 92% in Example 5, and 104% in Example 6.
[0052] [Table 1]
[0053] As a result, in Examples 1 to 3, almost no chipping or peeling occurred at the outer edge of the fourth antireflection film 8d, and the evaluation was excellent (A). In Examples 4 and 5, some chipping and peeling was observed at the outer edge of the fourth antireflection film 8d, but it was within the allowable range that does not cause practical problems, so the evaluation was good (B). The rate at which chipping and peeling occurred in Examples 1 to 3 was lower than the rate at which chipping and peeling occurred in Examples 4 and 5. In Example 6, chipping occurred at the outer edge of the fourth antireflection film 8d, but peeling did not occur, and therefore the evaluation was good (B). From the above, it has been found that the maximum value of the protrusion amount d is preferably 40% to 100% of the pixel size determined by the arrangement pitch P of the multiple photoelectric conversion elements 3, and most preferably 40% to 70%.
[0054] In this embodiment, the pitch between the convex portions of the lenses 7 and the arrangement pitch of the photoelectric conversion elements 3 are configured to match, but they may be partially or entirely different. When the pitch between the convex portions of the lenses 7 and the arrangement pitch of the photoelectric conversion elements 3 are different, the maximum value of the protrusion amount d of the fourth antireflection film 8d from the outer convex body 37 is 40% to 200% of at least one of the pixel size determined by the arrangement pitch of the multiple photoelectric conversion elements 3 and the pitch between the convex portions of the lenses 7.
[0055] Next, an example of a method for manufacturing the solid-state imaging element 1 according to this embodiment will be described, focusing on a method for manufacturing the outer periphery A2b of the peripheral light-shielding area A2. 8 to 14 are schematic diagrams showing an example of a method for manufacturing a solid-state imaging device according to an embodiment of the present invention.
[0056] To manufacture the solid-state imaging element 1, a semiconductor substrate 2 is prepared on which a plurality of photoelectric conversion elements 3 are formed. The plurality of photoelectric conversion elements 3, the peripheral circuits and wiring for extracting output from the photoelectric conversion elements 3, and the plurality of electrode pads formed on the semiconductor substrate 2 can be manufactured by a well-known semiconductor manufacturing process according to the type of solid-state imaging element 1.
[0057] 8, thereafter, a first planarization layer 4 is formed on the semiconductor substrate 2. The first planarization layer 4 can be formed, for example, by spin-coating a colorless and transparent acrylic resin solution onto the semiconductor substrate 2 to a thickness of about 0.1 μm, and then curing it by heat treatment. The first planarization layer 4 is formed over the entire surface of the semiconductor substrate 2 .
[0058] Thereafter, a resin layer including a filter portion 5, an inner light-shielding layer 15, and an outer light-shielding layer 25 is formed on the first planarization layer 4. In this embodiment, the filter portion 5, the inner light-shielding layer 15, and the outer light-shielding layer 25 are each composed of a red colored layer 5r, a green colored layer 5g, and a blue colored layer 5b, or a combination thereof. Therefore, each resin layer can be formed by patterning the colored layer required for each resin layer to the position, shape and thickness of each resin layer. Each colored layer can be formed by spin-coating a coloring material such as a pigment having the spectral transmittance characteristics and a photosensitive material containing an alkali-soluble resin on the first planarization layer 4, patterning the photosensitive material by a photolithography method including exposure and development steps, and curing the photosensitive material. The order of forming the red colored layer 5r, the green colored layer 5g, and the blue colored layer 5b is not particularly limited. However, in this embodiment, since the red colored layer 5r and the blue colored layer 5b are laminated in this order in the inner light-shielding layer 15, it is more preferable to form at least the red colored layer 5r before the blue colored layer 5b. When the filter portion 5, the inner light-shielding layer 15, and the outer light-shielding layer 25 are formed in this manner, the outer light-shielding layer 25 is formed on the first planarization layer 4 in the outer peripheral portion A2b, as shown in Fig. 8. For example, the outer light-shielding layer 25 is formed of a blue colored layer 5b. For this reason, the outer light-shielding layer 25 is formed simultaneously with the blue colored layer 5b of the filter portion 5 when the blue colored layer 5b of the filter portion 5 is formed. An outer peripheral surface 25a of the outer light-shielding layer 25 is formed in a substantially rectangular shape surrounding the outside of the filter portion 5 in a plan view.
[0059] Thereafter, a transparent resin layer 6A that forms a second planarization layer 6, a lens 7, an inner convex body 17, a flat resin layer 27, and an outer convex body 37 is formed on the resin layer including the filter portion 5, the inner light-shielding layer 15, and the outer light-shielding layer 25. In this embodiment, the lens 7, the inner convex body 17, the flat resin layer 27, and the outer convex body 37 are made of the same material, and therefore, hereinafter, the lens 7, the inner convex body 17, the flat resin layer 27, and the outer convex body 37 may be referred to as "lens 7, etc." When the second planarization layer 6 and the lenses 7, etc. are made of different materials, the transparent resin layer 6A is formed by a first layer and a second layer. In this case, the material forming the second planarization layer 6 is first applied and cured on each resin layer so that it has the thickness of the second planarization layer 6 when cured, thereby forming the first layer. After this, the material forming the lenses 7, etc. is applied and cured on the first layer so that it has a thickness that allows the lenses 7, etc. to be formed when cured, thereby forming the second layer. When the second planarization layer 6 and the lenses 7 and the like are made of the same material, the transparent resin layer 6A is formed into a single layer having a thickness sufficient for forming the second planarization layer 6 and the lenses 7 and the like when cured. The transparent resin layer 6A can be formed by spin-coating a transparent resin that forms the transparent resin layer 6A. According to such a forming method, the transparent resin layer 6A is formed on the surfaces of the filter portion 5, the inner light-shielding layer 15, and the outer light-shielding layer 25 and on the first planarization layer 4 on the outer side thereof.
[0060] Thereafter, the lens 7, the inner convex body 17, the flat resin layer 27, and the outer convex body 37 are formed on the surface of the transparent resin layer 6A. In this embodiment, the inner convex body 17, the flat resin layer 27, and the outer convex body 37 are formed at the same time as the lens 7 by the same manufacturing method. An example in which the lens 7 is formed by transfer type will be described below. 9, a resist material 7A made of a photosensitive resin material having alkali solubility, photosensitivity, and thermal flow properties is laminated on the transparent resin layer 6A to form a lens formation layer. Then, a photomask M is placed on the resist material 7A, and the resist material 7A is exposed to light. Here, the photomask M has an exposure pattern formed thereon for dividing the lens formation layer and forming, in the lens formation layer, shapes corresponding to the lenses 7, the inner convex body 17, the flat resin layer 27, and the outer convex body 37. The photomask M is positioned and aligned with the semiconductor substrate 2 so that each lens 7 faces each photoelectric conversion element 3.
[0061] Fig. 10 shows an example of a photomask M for forming the flat resin layer 27 and the outer convex body 37 in the outer peripheral portion A2b. Fig. 10 shows a region corresponding to the portion F5 in Fig. 1. The photomask M has a mask pattern M37 formed thereon for removing unnecessary portions of the resist material 7A in order to form the outer convex body 37. Although not particularly shown, a mask pattern for removing unnecessary portions of the resist material 7A in order to form the lens 7 is formed in the effective light-receiving area A1. In this embodiment, the mask pattern for forming the lens 7 and the mask pattern M37 are the same pattern except that they are formed at different locations. The mask pattern M37 is formed so as to cover the range from the vicinity of the outer circumferential surface 15a to the vicinity of the outer circumferential surface 25a. The inner periphery Ma of the mask pattern M37 forms the inner periphery of the outer convex body 37. The inner periphery Ma is formed in a position where three or more outer convex bodies 37 are formed, inside the line to be removed L that forms the outer edge of the fourth antireflection film 8d. Note that, although in this embodiment, three or more outer convex bodies 37 are arranged side by side, from the viewpoint of preventing peeling, it is sufficient that two or more are arranged side by side. In contrast to this, the outer periphery Mb of the mask pattern M37 is formed so as to cover the area outside the lines L to be removed.
[0062] Thereafter, with the photomask M in place, the resist material 7A is exposed to light. At this time, the mask pattern M37 is formed in a range covering the inner light-shielding layer 15 and the outer light-shielding layer 25. Therefore, the inner light-shielding layer 15 and the outer light-shielding layer 25 are disposed under the transparent resin layer 6A. The outer light-shielding layer 25 has a step adjustment function that makes the surface of the transparent resin layer 6A in the peripheral light-shielding region A2 the same height as the transparent resin layer 6A in the light-receiving effective region A1 when exposing the resist material 7A. This allows the shape of the outer convex body 37 to be exposed in the same way as the lens 7 with the focus setting in the light-receiving effective region A1, so that the shape of the outer convex body 37 can be well exposed. For example, if the outer light-shielding layer 25 is not provided, the exposure light is defocused in the peripheral light-shielding region A2, so that the shape of the outer convex body 37 may not be resolved. Furthermore, the outer light-shielding layer 25 has the effect of attenuating the exposure light that reaches the semiconductor substrate 2, is reflected, and re-enters the transparent resin layer 6A. Therefore, the shape of the outer convex body 37 can be favorably formed in that overexposure due to reflected light from the semiconductor substrate 2 is suppressed.
[0063] Thereafter, the exposed resist material 7A is developed to remove unnecessary resist material 7A. As a result, the resist material 7A is patterned, and shapes roughly corresponding to the lens 7, the inner convex body 17, the flat resin layer 27, and the outer convex body 37 are formed on the surface of the resist material 7A. Thereafter, the resist material 7A is heated by thermal flow, and a matrix shape corresponding to the lens 7, the inner convex body 17, the flat resin layer 27, and the outer convex body 37 is formed on the surface of the resist material 7A. Thereafter, the matrix shape formed in the resist material 7A is transferred to the transparent resin layer 6A by dry etching, and the uneven portion including the lenses 7, inner convex bodies 17, flat resin layer 27, and outer convex bodies 37 is formed. 11, for example, the outer peripheral portion A2b is formed with the second planarization layer 6 and an uneven portion including the outer convex body 37 and the flat resin layer 27 formed on the second planarization layer 6. The effective light-receiving area A1 and the inner peripheral portion A2a in its vicinity are formed with an uneven portion including the lens 7 and the inner convex body 17.
[0064] 12, an anti-reflection film 8 is formed on the surface of the transparent resin layer 6A on which the uneven shape of the lenses 7 and the like is formed. For example, a thin film of silicon dioxide is formed as the anti-reflection film 8 by using CVD (chemical vapor deposition). The anti-reflection film 8 curves along the uneven shape of the surface of the transparent resin layer 6A. Therefore, the surface of the anti-reflection film 8 has a curved surface and a flat surface that follow the uneven shape of the transparent resin layer 6A. The anti-reflection film 8 is formed on the entire surface of the transparent resin layer 6A.
[0065] In the above manufacturing process, the first planarization layer 4, the transparent resin layer 6A, and the anti-reflection film 8 are laminated in this order on the substrate outer peripheral region A3. Therefore, the scribe S and the electrode pads 9 on the substrate outer peripheral region A3 are also covered with the first planarization layer 4, the transparent resin layer 6A, and the anti-reflection film 8. Therefore, the first planarization layer 4, the transparent resin layer 6A, and the anti-reflection film 8 on the scribe S and the electrode pad 9 are removed. 13, a mask 50 is placed on the anti-reflection film 8 inside the line to be removed L, and the anti-reflection film 8 outside the mask 50 is removed by dry etching. The type of dry etching is selected from an appropriate type capable of etching the material of the anti-reflection film 8. For example, when the anti-reflection film 8 is made of silicon dioxide, reactive dry etching using, for example, fluorine gas as the etching gas may be used. As a result, the antireflection film 8 on the outer side of the mask 50 is removed to form the outer edge of the fourth antireflection film 8d. The surface of the outer convex body 37 is exposed on the transparent resin layer 6A from which the antireflection film 8 has been removed.
[0066] 14, the transparent resin layer 6A outside the mask 50 is removed by dry etching. The type of dry etching is selected from among those that can etch the material of the transparent resin layer 6A. For example, when the transparent resin layer 6A is made of an organic resin, reactive dry etching using oxygen gas as the etching gas may be used. In the reactive dry etching, as the etching progresses, the etching gas also reaches the lower surface side of the fourth antireflection film 8d, so that the side surface of the transparent resin layer 6A on the outer light-shielding layer 25 is also gradually etched. Therefore, while the transparent resin layer 6A on the outer light-shielding layer 25 is being removed, a part of the transparent resin layer 6A on the lower surface of the outer edge of the fourth antireflection film 8d is also removed. As a result, a protruding portion 8e that protrudes outward beyond the outer circumferential surface E is formed.
[0067] When the transparent resin layer 6A is etched, the outer light-shielding layer 25 and the first planarization layer 4 are also etched. When the anti-reflection film 8, the transparent resin layer 6A, and the first planarization layer 4 are removed, the scribe S and the surface of the semiconductor substrate 2 are exposed, and the electrode pads 9 are also exposed. For this reason, it is possible to perform a continuity test using the electrode pads 9. In this manner, a plurality of solid-state imaging elements 1 are formed in the area surrounded by the scribe lines S on the silicon wafer W. Thereafter, for example, a cleaning step is performed, and the scribe lines S are cut to produce a plurality of solid-state imaging elements 1.
[0068] According to the solid-state imaging device 1 of this embodiment, a fourth anti-reflection film 8d having unevenness in the thickness direction is formed on the outer periphery of the anti-reflection film 8. A protruding portion 8e that protrudes from the outer convex body 37 and the outer periphery E of the second planarization layer 6 is formed on the outer edge of the fourth anti-reflection film 8d during the etching process of the transparent resin layer 6A. However, since the protruding portion 8e is a part of the fourth anti-reflection film 8d having an uneven shape, it has a larger moment of area second than a flat plate. Therefore, even if an external force acts on the protruding portion 8e during, for example, a cleaning process, it is difficult to peel off. By setting the protruding amount of the protruding portion 8e to be at most 40% to 200% of the arrangement pitch of the outer convex bodies 37, the protruding portion 8e becomes even more unlikely to peel off.
[0069] The operation of this embodiment will be described in comparison with a comparative example. 15 and 16 are schematic diagrams showing a method for manufacturing a solid-state imaging device of a comparative example, and Figs. 17 and 18 are cross-sectional views showing examples of damage forms of the solid-state imaging device of the comparative example.
[0070] The solid-state imaging element of the comparative example is manufactured in the same manner as in this embodiment, except that a flat resin layer 27 is formed in place of the outer convex body 37 on the outer periphery A2b. 15, after the antireflection film 8 is formed, a flat resin layer 27 is formed on the transparent resin layer 6A in the outer circumferential portion A2b. Since the antireflection film 8 is formed along the surface of the flat resin layer 27, the photoelectric conversion element 3 in the outer circumferential portion A2b is composed only of the flat third antireflection film 8c. Thereafter, the anti-reflection film 8 and the transparent resin layer 6A are sequentially etched in the same manner as in this embodiment, thereby obtaining the solid-state imaging element 100 of the comparative example shown in FIG. In the solid-state imaging element 100, the outer edge of the third antireflection film 8c is formed along the line to be removed L, and a protruding portion 8f protruding from the outer circumferential surface E of the transparent resin layer 6A is formed. Since the protruding portion 8f is a thin plate-like film, its area moment of inertia is much smaller than that of the protruding portion 8e, and therefore it is much easier to break than the protruding portion 8e.
[0071] 17, when an external force f acting toward the semiconductor substrate 2 acts on the tip of the protrusion 8f, the protrusion 8f breaks at the base end of the protrusion 8f. The broken portion of the protrusion 8f turns into fragments F1 and scatters onto the solid-state imaging element 100. The fragments F1 rub against the surface of the solid-state imaging element 100 and may damage the surface of the solid-state imaging element 100. If the surface of the solid-state imaging element 100 is damaged, there is a risk that a defect will occur in the solid-state imaging element 100. 18, if the adhesion between the third antireflection film 8c and the transparent resin layer 6A in the vicinity of the outer peripheral surface E is too low, when an external force f acts on the protruding portion 8f, the third antireflection film 8c in the vicinity of the outer peripheral surface E may peel off from the surface of the transparent resin layer 6A, and the third antireflection film 8c may break inside the outer peripheral surface E. In this case, the broken third antireflection film 8c, together with the protruding portion 8f, becomes fragments F2 and scatters onto the solid-state imaging element 100. The fragments F2 may rub against the surface of the solid-state imaging element 100 and damage the surface of the solid-state imaging element 100. In this embodiment, the fourth antireflection film 8d located inside the protrusion 8e is in close contact with at least three or more outer convex bodies 37, and therefore has a wide contact area with the surface of the outer convex body 37, making it difficult for the fourth antireflection film 8d to be sheared along the surface of the outer convex body 37. For this reason, peeling is also difficult to occur near the outer circumferential surface E.
[0072] In the comparative example, it is also possible to prevent the protrusion 8f from being formed in order to prevent damage to the third antireflection film 8c. For example, after etching of the third antireflection film 8c is completed, a protective resin layer 101 (see the two-dot chain line in FIG. 16) is formed on the outer edge of the third antireflection film 8c and on the semiconductor substrate 2 on the outer side thereof to protect the third antireflection film 8c and the outer peripheral surface E formed below the third antireflection film 8c. For example, the protective resin layer 101 can be formed by photolithography using a transparent resin similar to that of the transparent resin layer 6A. However, the manufacturing method of this comparative example requires the addition of manufacturing steps of forming and removing the protective resin layer, which increases the manufacturing process, resulting in increased manufacturing time and costs compared to this embodiment.
[0073] As described above, according to the solid-state imaging element 1 of this embodiment, the fourth antireflection film 8d has an uneven shape that conforms to the surface of the outer convex body 37, thereby preventing damage (including peeling and chipping) at the outer edge of the antireflection film 8. According to the manufacturing method of this embodiment, the outer convex body 37 can be manufactured in the same manufacturing process as the lens 7, in the same manner as the lens 7, so that a solid-state imaging element 1 capable of preventing damage to the outer edge of the anti-reflection film 8 can be efficiently manufactured.
[0074] In the above embodiment, an example has been described in which the outer convex body 37 is formed in the same shape as the lens 7. However, the shape of the outer convex body 37 is not limited to the same shape as the lens 7, as long as an uneven shape can be formed on the fourth antireflection film 8d. In other words, since the outer convex body 37 does not require a light collecting function, it does not have to be the same shape as or similar to the shape of the convex lens surface of the lens 7. The uneven shape of the outer convex body 37 may be a shape that does not function as a lens. For example, the outer convex body 37 may be formed at a pitch different from the arrangement pitch of the lenses 7. For example, when the lenses 7 are formed at a pitch of 0.8 μm, the outer convex body 37 may be formed at a larger pitch, such as a pitch of 1.0 μm. For example, the outer convex body 37 may have a convex shape different from the convex lens shape of the lenses 7 while having the same arrangement pitch as the lenses 7 .
[0075] In the above embodiment, an example has been described in which the outer convex bodies 37 are formed in a rectangular lattice pattern similar to that of the lenses 7. However, the arrangement of the outer convex bodies 37 may be different from the arrangement of the lenses 7. For example, the outer convex bodies 37 may be in a staggered arrangement or a diagonal lattice arrangement in which the rows from the inner periphery to the outer periphery are shifted by less than the respective arrangement pitches.
[0076] In the above embodiment, an example has been described in which the inner convex body 17 is provided. However, in the case where cracks do not occur on the outer edge of the lens 7, the inner convex body 17 may be omitted.
[0077] In the above embodiment, the planar shape of the outer convex body 37 has been described as being close to a square or circle, similar to the lens 7. However, the outer convex body 37 may include a dome-shaped convex portion that is elongated in one direction. In this case, the longitudinal direction of the dome-shaped convex portion may be substantially perpendicular to the outer edge of the fourth antireflection film 8d.
[0078] In the above embodiment, the filter unit of the solid-state imaging device separates the incident light into red, green, and blue colors. However, the color separation of the filter unit is not limited to this. For example, the filter unit may separate the incident light into cyan, magenta, and yellow colors.
[0079] In the above embodiment, the solid-state imaging element 1 is described as a color imaging element. However, the solid-state imaging element may be a monochrome imaging element. In this case, the filter unit may be a filter other than a color filter, such as an infrared cut filter.
[0080] 6, the outer light-shielding layer 25 is disposed below (on the substrate side) the fourth antireflection film 8d, but the outer light-shielding layer 25 does not necessarily have to be disposed. That is, instead of the outer light-shielding layer 25, the region corresponding to the fourth antireflection film 8d may be filled with the same material as the second planarization layer 6, and the region corresponding to the third antireflection film 8c may be provided with a blue colored layer. In addition, instead of the outer light-shielding layer 25, a blue colored layer may be provided in the area corresponding to the fourth anti-reflection film 8d, and a red colored layer and a blue colored layer may be laminated in this order in the area corresponding to the third anti-reflection film 8c.
[0081] The outer convex body 37 may be rectangular. That is, the cross-sectional shape of the outer convex body 37 is semicircular with a curved surface as shown in Fig. 6, but the upper end surface may be a straight line. However, there is a valley between adjacent outer convex bodies 37. Furthermore, compared to when the radius of curvature of the curved surface of the protrusion 8e is large, it is preferable that the radius of curvature of the curved surface of the protrusion 8e is small, since this increases the moment of inertia of area and makes the protrusion 8e less likely to break (chip).
[0082] Moreover, although the protruding portion 8e has been shown to have a curved shape as an example, it may have a linear shape. 14, the protrusion 8e faces downward (toward the semiconductor substrate 2), but may face upward. In order to form the protrusion 8e facing upward, it is possible to manufacture the protrusion 8e by changing the size of the mask 50. However, it is preferable that the protrusion 8e faces downward because it is easier to withstand an external force when the external force is applied.
[0083] Although the preferred embodiment of the present invention has been described above, the present invention is not limited to the embodiment. Addition, omission, substitution, and other modifications of the configuration are possible without departing from the spirit of the present invention. Furthermore, the present invention is not limited by the foregoing description, but only by the scope of the appended claims. [Industrial Applicability]
[0084] According to the solid-state imaging device of the present invention, peeling of the antireflection film at the outer edge can be prevented. According to the method for manufacturing a solid-state imaging device of the present invention, it is possible to efficiently manufacture a solid-state imaging device capable of preventing peeling of the outer edge of the antireflection film. [Explanation of symbols]
[0085] 1. Solid-state imaging element 2. Semiconductor Substrate 3 Photoelectric conversion element 4 First planarization layer 5 Filter section 5b Blue colored layer 5g green colored layer 5r red colored layer 6 Second planarization layer 6A Transparent resin layer 7 Lenses 8 Anti-reflection coating 8a 1st anti-reflection coating 8b Second anti-reflection coating 8c Third anti-reflection coating 8d 4th anti-reflection coating 8e Protrusion 9 Electrode Pads 15 Inner light shielding layer 17 Inner convex body 25 Outer light shielding layer (light shielding layer) 27 Flat resin layer 37 Outer convex body (convex part, resin layer) A1 Effective light receiving area A2 Peripheral light shielding area A2a Inner circumference A2b outer periphery A3 Board outer area E Outer surface M Photomask
Claims
1. A substrate; A plurality of photoelectric conversion elements arranged on the substrate; a filter section arranged above the plurality of photoelectric conversion elements and transmitting light incident on the plurality of photoelectric conversion elements; A plurality of lenses disposed above the filter unit; a resin layer disposed so as to surround from the outside the outer edges of the plurality of lenses in a plan view; an anti-reflection film formed on the plurality of lenses and the resin layer, the anti-reflection film has a peripheral film covering a peripheral portion of the resin layer in a plan view, the outer circumferential portion of the resin layer has a lens shape, On the substrate, there are provided an effective light-receiving area (A1), a peripheral light-shielding area (A2) adjacent to an outer edge of the effective light-receiving area (A1), and a substrate outer periphery area (A3) which is an area from the outer edge of the peripheral light-shielding area (A2) to an outer edge of the substrate, the peripheral film has an uneven shape having unevenness following the lens shape in a thickness direction of the resin layer, at least a part of an outer edge of the peripheral film has a protruding portion that protrudes outward beyond the resin layer, and the protruding portion is curved in the thickness direction following the lens shape in the substrate peripheral region (A3); In the substrate peripheral region (A3), an electrode pad is formed on the substrate, The protrusion is provided in a region of the substrate outer periphery region (A3) where the electrode pads are not provided, protruding from an outer edge of the peripheral light-shielding region (A2) in a plan view of the resin layer. Solid-state imaging element.
2. A light-shielding layer that absorbs external light is further provided between the substrate and the resin layer, The filter portion has a plurality of colored layers, At least a part of the light-shielding layer is formed of the colored layer. The solid-state imaging device according to claim 1 .
3. 3. The solid-state imaging device according to claim 1, wherein a maximum amount of protrusion of said outer peripheral film from said resin layer is 40% or more and 200% or less of a pixel size determined by an arrangement pitch of said plurality of photoelectric conversion elements.
4. The uneven shape of the outer peripheral film has two or more convex portions in a direction from an outer edge of the resin layer toward an inside thereof.
4. The solid-state imaging device according to claim 1.
5. The uneven shape of the outer peripheral film has an arrangement pitch of convex portions of the uneven shape that is equal to an arrangement pitch of the plurality of lenses.
5. The solid-state imaging device according to claim 1.
6. the anti-reflection coating has an inner coating formed on the plurality of lenses and an intermediate coating disposed between the inner coating and the outer peripheral coating, The intermediate film is formed flat.
6. The solid-state imaging device according to claim 1.
7. Preparing a substrate on which a plurality of photoelectric conversion elements are formed; forming a filter portion covering the plurality of photoelectric conversion elements above the plurality of photoelectric conversion elements; forming a resin layer on the filter portion; forming, on the resin layer, a plurality of lenses covering the plurality of photoelectric conversion elements on the filter portion, and a lens shape having irregularities in a thickness direction on an outer periphery of the resin layer in a plan view, by patterning the resin layer; forming an anti-reflective film on a surface of the patterned resin layer; removing a portion of the antireflection film and the resin layer by etching the outer edge of the antireflection film and the outer periphery of the resin layer over the entire circumference such that at least a portion of the outer edge of the antireflection film protrudes from the resin layer and is curved in the thickness direction following the shape of the lens; On the substrate, there are provided an effective light-receiving area (A1), a peripheral light-shielding area (A2) adjacent to an outer edge of the effective light-receiving area (A1), and a substrate outer periphery area (A3) which is an area from the outer edge of the peripheral light-shielding area (A2) to an outer edge of the substrate, In the substrate peripheral region (A3), an electrode pad is formed on the substrate, At least a part of an outer edge of the anti-reflection film protrudes from an outer edge of the peripheral light-shielding region (A2) into an area of the substrate outer periphery region (A3) where the electrode pads are not provided, in a plan view of the resin layer. A method for manufacturing a solid-state imaging device.
Citation Information
Patent Citations
Manufacture of semiconductor device such as solid-state image pickup device
JP2000164836A
Solid state imaging device
JP2013012518A
Manufacturing method of color solid-state image sensor
JP2013131613A
Solid state image sensor
JP2014103299A
Solid-state imaging element including microlens layer with dummy structure
JP2018207086A