Heat-resistant carbide layer

The CVD method with a specific C/Si molar ratio and aromatic carbon source achieves highly oriented silicon carbide coatings with enhanced mechanical and chemical properties, addressing the inefficiencies of existing methods in producing stable and uniform refractory carbide layers for larger surfaces.

JP7594117B2Active Publication Date: 2024-12-03SGL CARBON SE
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023535034
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-12-09
Filing Date
2021-12-09
Publication Date
2024-12-03
Estimated Expiration
2041-12-09

AI Technical Summary

Technical Problem

Existing chemical vapor deposition (CVD) methods for refractory carbides, such as silicon carbide (SiC), struggle to produce coatings with high mechanical stability and etch resistance efficiently, particularly for larger surfaces, and often result in non-uniform crystal orientations that affect their performance.

Method used

A CVD method using a gas mixture with a specific C/Si molar ratio of 0.85 to 1.45, including an aromatic carbon source, is employed to form silicon carbide crystals with a preferred {111} orientation, resulting in a highly oriented and uniform layer with enhanced mechanical and chemical properties.

Benefits of technology

The method produces silicon carbide coatings with high hardness, thermal shock resistance, and corrosion resistance, suitable for large-scale production and application on various substrates, including wafer carriers, by optimizing reaction conditions to achieve uniform {111} orientation and improved mechanical stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007594117000010
    Figure 0007594117000010
  • Figure 0007594117000011
    Figure 0007594117000011
  • Figure 0007594117000012
    Figure 0007594117000012
Patent Text Reader

Abstract

The present disclosure relates to a novel CVD method for preparing layers comprising refractory carbide crystals, to the layers obtainable by said method, and to their various uses and applications.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a novel CVD method for preparing layers comprising refractory carbide crystals, to the layers obtainable by said method and their various uses and applications, for example deposited on wafer carriers. [Background technology]

[0002] Graphite parts coated with refractory carbides, especially silicon carbide (SiC), are commonly used, for example, in the manufacture of LEDs (light emitting diodes) and in semiconductor processing. Because these processes require high purity parts, refractory coatings are commonly applied using chemical vapor deposition (CVD). In CVD, a carrier gas (e.g., H) is used to deposit the SiC layer. 2 ) and precursor gas (SiCl 4 +CH 4 A gas mixture containing precursors such as benzene, benzene, and benzene-1, is fed into a reactor heated to a temperature in excess of 1000° C., where the precursors react chemically to form solid SiC on the surface of the deposited graphite component. Commonly used precursors for CVD of SiC on graphite components are short-chain hydrocarbons such as methane (CH 4 ), ethylene (C 2 H 4 ), propane (C 3 H 8 ) and silicon tetrachloride (SiCl 4 ) and methyltrichlorosilane (Cl 3 SiCH 3 , "MTS").

[0003] The CVD process results in a specific crystal structure in the SiC coating (usually β-SiC, also referred to as 3C-SiC). The crystals may be randomly oriented in the coating or oriented in a preferred direction. The orientation is the result of complex interactions during the SiC growth. Typically, SiC crystals deposited on a substrate (e.g., graphite or silicon) do not show a strong preferred orientation or are oriented with the (220) plane of the SiC crystal parallel to the substrate surface ("(220) orientation"). Past attempts to improve refractory carbide coatings have focused on the XRD (X-ray diffraction) characteristics of the refractory carbides, as will be appreciated from the prior art listed below.

[0004] Non-Patent Document 1 describes the chemical vapor deposition (CVD) of halides. <110> Ultrafast fabrication of oriented β-SiC is described. Chemical vapor deposition of halides is performed using silicon tetrachloride (SiCl 4 ) and methane (CH 4 ) as a precursor. The surface morphology of β-SiC films prepared at an ultra-high deposition temperature of 1773 K and a total pressure of 40 kPa results in a hexagonal structure that appears to contain large hexagonal crystals. The drawing shows that the distance from one corner of a hexagon to its opposite corner is many times 5 μm.

[0005] Non-Patent Document 2 describes the high-speed deposition of thick SiC films using halide precursors. 4 ) and methane (CH 4 The film deposited at 1573K using ) as a precursor showed strong <111> indicating a preferred orientation. Nevertheless, the XRD pattern of the β-SiC film prepared at 1573 K has a prominent (220) diffraction peak. The surface morphology of the β-SiC film deposited at 1573 K has been described as exhibiting pyramidal structures with six-fold symmetry. However, the hexagons depicted in one SEM image do not appear to fit the corresponding grains.

[0006] Non-Patent Document 3 describes the preparation of ultra-thick β-SiC films by chemical vapor deposition of halides.4 as a silicon source, and methane (CH 4 ), acetylene (C 2 H 2 ), propane (C 3 H 8 ), and liquefied petroleum gas were used as carbon sources, respectively. 4 It has been reported that only {111} peaks were identified in XRD after CVD under certain conditions, including. In the low deposition temperature range (<1473 K), the morphology of the β-SiC films shows a smooth layered structure. In the high deposition temperature range (1573-1773 K), cauliflower-like crystals, rounded hillock-like crystals, and multiply twinned crystals were obtained using different carbon sources.

[0007] In Non-Patent Document 4, SiC coatings were produced on carbon / carbon (C / C) composite substrates using chemical vapor deposition (CVD) at various temperatures (1100°C, 1200°C, 1300°C). 3 SiCl 3 )-H 2 -Ar gas system is used for the chemical reaction. All X-ray diffraction patterns of SiC coatings produced at various deposition temperatures have a strong (220) reflection, which indicates a specific preferential orientation only for the (111) orientation. Although a well-developed faceted structure is stated to be obtained for the coatings produced at 1200 °C, SEM images show a high degree of heterogeneity of the crystal surface overall. The authors also investigated the mechanical properties and concluded that the (111) texture plays a key role in determining the mechanical properties, while the grain size, crystallinity, and stacking fault density are less important. The highest hardness values ​​(41 ± 2 GPa) were observed for the coatings produced at 1200 °C.

[0008] Non-Patent Document 5 describes a number of SiC coatings, each formed by MTS under different conditions. Many of the coatings deposited at low deposition temperatures show a preferred orientation plane (tri-index) of (111). In run 71, with a deposition temperature of 1400 °C, crystals with hexagonal cross sections were accidentally obtained.

[0009] In Non-Patent Document 6, MTS and H on graphite are 2 It has been shown that a (110) preferred orientation can be obtained in SiC coatings from and when the precursors in the gas phase are partially depleted. The structural resolution of the SiC surface is insufficient to conclude specific structural surface features such as polygonal shapes.

[0010] Non-Patent Document 7 describes the preparation of highly oriented β-SiC bulk bodies by halide laser chemical vapor deposition. A single surface SEM image of a bulk body prepared at 10 kPa total pressure and a deposition temperature of 1573 K shows a large hexagonal symmetric surface morphology with a crystal cross-sectional diameter of approximately 50 μm. The hardness is only approximately 33 GPa. Another recent publication, Non-Patent Document 8, describes fine-grained 3C-SiC thick films prepared by hybrid laser chemical vapor deposition, improving the Vickers microhardness value of the 3C-SiC thick films from 30 GPa to 35 GPa.

[0011] Although useful puncturability of refractory carbide layers appears to be achieved in some cases by laser CVD, the method cannot be adapted to efficiently coat larger surfaces.

[0012] In the CVD method disclosed in Non-Patent Document 9, gaseous SiO is reacted with toluene vapor to generate SiC in the presence of iron oxide as a catalytic component. This method is experimental, and the resulting coating is not endowed with a specific preferential SiC crystal orientation as evidenced in the XRD pattern. Furthermore, this method produces fibrous by-products and results in coatings containing Fe, which may not be suitable for many commercial settings.

[0013] There is an unmet need for a refractory carbide layer that can be produced in an efficient process and that provides very high mechanical stability and etch resistance. [Prior art documents] [Non-patent literature]

[0014] [Non-Patent Document 1] Tu et al., J. Am. Ceram. Soc., 99 [1] 84-88 (2016) [Non-Patent Document 2] Han et al., Key Engineering Materials Vol. 616 (2014) pp 37-42 [Non-Patent Document 3] Tu et al., Materials Research Innovations, 2015, 19, 397-402 [Non-Patent Document 4] Long et al., International Journal of Applied Ceramic Technology, Vol. 10, No. 1, p. 11-19 (2013) [Non-Patent Document 5] Chin et al., Thin Solid Films, 40 (1977) 57-72 [Non-Patent Document 6] Kim et al., Thin Solid Films 266 (1995) 192-197 [Non-Patent Document 7] Cheng et al., Journal of the European Ceramic Society 37 (2017) 509-515 [Non-Patent Document 8] Lai et al., Journal of the American Ceramic society, 2019, 1-11 [Non-Patent Document 9] Murakawa et al., Journal of the Ceramic Society of Japan 125 (2017) 85-87 Summary of the Invention [Problem to be solved by the invention]

[0015] SUMMARY OF THE DISCLOSURE The present disclosure is directed to addressing one or more of the problems set forth above. [Means for solving the problem]

[0016] In a first aspect, the present disclosure relates to a chemical vapor deposition (CVD) method for preparing a layer comprising silicon carbide crystals, at least a portion of which is formed from a gas mixture comprising a silicon source and an aromatic carbon source, the gas mixture having a C / Si molar ratio of about 0.85 to about 1.45, more particularly about 0.9 to about 1.3, and especially about 1.0 to about 1.2.

[0017] In some embodiments, the aromatic carbon source is 6 ~C 30 In some embodiments, the aromatic compound may be benzene, C 1 ~C 6 Alkylbenzene, C 1 ~C 6 Dialkylbenzene, C 1 ~C 6 Trialkylbenzene, C 1 ~C 6 The aromatic compound may be selected from tetraalkylbenzenes, biphenyl derivatives, diphenylmethane derivatives, and naphthalene derivatives, and more specifically, may be a compound selected from benzene, toluene, ethylbenzene, p-xylene, o-xylene, m-xylene, mesitylene, durene, 2-phenylhexane, biphenyl, diphenylmethane, and naphthalene, and in particular may be toluene.

[0018] In some embodiments, the reaction temperature can be from about 900°C to about 1800°C, more specifically from about 1000°C to about 1400°C, and more specifically from about 1100°C to about 1200°C.

[0019] In some embodiments, the reaction may be carried out under reduced pressure, specifically between about 0 mbar and about 300 mbar, more specifically between about 50 mbar and about 200 mbar, and more specifically between about 75 mbar and about 150 mbar. 2 In some embodiments, the molar ratio of the inert carrier gas to Si is about 10 to about 40, more specifically about 15 to about 35, and particularly about 20 to about 30.

[0020] In some embodiments, the method may result in a free-standing layer. In some embodiments, the method may comprise depositing said layer on a carbonaceous substrate such as graphite, in particular a wafer carrier comprising graphite, or on a silicon based substrate, a semiconductor comprising silicon such as a wafer, or on a layer comprising a refractory metal carbide such as silicon carbide.

[0021] In a second aspect, the present disclosure relates to a layer comprising silicon carbide crystals, the layer being produced or producible by the method according to the first aspect of the present disclosure, wherein upon SEM image analysis of a cross-section of the layer, approximately 20% or less of the area of ​​the cross-section has a pattern of parallel lines inclined by more than 15° relative to the portion of the surface of the layer nearest the respective image.

[0022] In some embodiments, the surface of the layer may comprise regular hexagonal pyramidal silicon carbide crystal apexes, with less than 10% of the surface being occupied by large regular hexagonal pyramidal crystal apexes having a distance from one corner of the apex's regular hexagonal base to the opposite corner of the base of about 25 μm or more. Additionally or alternatively, the layer may be characterized by a Raman spectrum of the layer having two overlapping peaks, the first of which is at 758 cm. -1 ~778cm -1 The second peak is at 785 cm-1 ~805cm -1 and an area ratio calculated by dividing the first area of ​​the first peak by the second area of ​​the second peak is equal to or greater than about 0.05.

[0023] In some embodiments, 10% or more of the surface of the layer may be covered by the apex of the regular hexagonal pyramid shape.

[0024] In some embodiments, the layer may have a distribution of silicon carbide crystal orientations such that the orientation quality Q is greater than or equal to about 0.90, particularly greater than or equal to about 0.95, more particularly greater than or equal to 0.97, in particular greater than or equal to about 0.99, calculated from the maximum peak intensity of an X-ray diffractogram detected with CuKα radiation at a wavelength of 1.5406 Å according to the following formula: Q=(I 111 +I 222 +I 333 / 511 ) / (I 111 +I 200 +I 220 +I 311 +I 222 +I 400 +I 331 +I 420 +I 333 / 511 +I 422 ) During the ceremony, I 111 is the maximum intensity at 2θ in the range of 34.6° to 36.6°, I 200 is the maximum intensity at 2θ in the range of 40.4° to 42.4°, I 220 is the maximum intensity at 2θ in the range of 59.0° to 61.0°, I 311 is the maximum intensity at 2θ in the range of 70.8° to 72.8°, I 222 is the maximum intensity at 2θ in the range of 74.5° to 76.5°, I 400 is the maximum intensity at 2θ in the range of 89.0° to 91.0°, I 331is the maximum intensity at 2θ in the range of 99.8° to 101.8°, I 420 is the maximum intensity at 2θ in the range of 103.4° to 105.4°, I 333 / 511 is the maximum intensity at 2θ in the range of 132.4° to 134.4°, I 422 is the maximum intensity at 2θ in the range of 119.0° to 121.0°.

[0025] In some embodiments, the surface of the layer may have a mean linear intercept surface grain size in the range of about 0.2 μm to about 25 μm, more specifically about 0.4 μm to about 10 μm, and particularly about 0.6 μm to about 5 μm.

[0026] In some embodiments, the surface hardness of said layer is at least about 0.5% greater than the cross-sectional hardness of said layer, more particularly at least about 1% greater, especially at least about 2% greater.

[0027] In some embodiments, the average roughness Ra according to ISO 4287 of a surface of the layer may be in the range of about 0.01 nm to about 100 nm, more particularly about 0.2 nm to about 50 nm, in particular about 0.4 nm to about 25 nm (nanoscale roughness). Additionally or alternatively, the average roughness Ra according to ISO 4287 of a surface of the layer may be in the range of about 100 nm to about 10 μm, more particularly about 200 nm to about 8 μm, in particular about 300 nm to about 6 μm (microscale roughness).

[0028] In some embodiments, the layer may have a thickness of about 0.5 μm or more, more particularly about 1 μm or more, especially about 10 μm or more.

[0029] In a third aspect of the present disclosure, there is provided a layer comprising silicon carbide crystals, the distribution of silicon carbide crystal orientation being such that an orientation quality Q is greater than or equal to about 0.90, particularly greater than or equal to about 0.95, more particularly greater than or equal to about 0.97, in particular greater than or equal to about 0.99, the orientation quality Q being calculated from the maximum peak intensity of an X-ray diffractogram detected with CuKα radiation at a wavelength of 1.5406 Å according to the following formula: Q=(I 111 +I 222 +I 333 / 511 ) / (I 111 +I 200 +I 220 +I 311 +I 222 +I 400 +I 331 +I 420 +I 333 / 511 +I 422 ) During the ceremony, I 111 is the maximum intensity at 2θ in the range of 34.6° to 36.6°, I 200 is the maximum intensity at 2θ in the range of 40.4° to 42.4°, I 220 is the maximum intensity at 2θ in the range of 59.0° to 61.0°, I 311 is the maximum intensity at 2θ in the range of 70.8° to 72.8°, I 222 is the maximum intensity at 2θ in the range of 74.5° to 76.5°, I 400 is the maximum intensity at 2θ in the range of 89.0° to 91.0°, I 331 is the maximum intensity at 2θ in the range of 99.8° to 101.8°, I 420 is the maximum intensity at 2θ in the range of 103.4° to 105.4°, I 333 / 511 is the maximum intensity at 2θ in the range of 132.4° to 134.4°, I 422 is the maximum intensity at 2θ in the range of 119.0° to 121.0°.

[0030] In some embodiments, the layer may be provided with features as described in the second aspect of the present disclosure.

[0031] In a fourth aspect, the present disclosure relates to a device, in particular a wafer carrier, for high temperature applications. The device comprises a layer according to the second or third aspect of the present disclosure. The layer is provided on a surface of the device.

[0032] In a fifth aspect, the present disclosure relates to the use of a layer according to the second or third aspect of the present disclosure for supporting a semiconductor. [Brief description of the drawings]

[0033] [Figure 1] 1 shows a scanning electron microscope (SEM) image of the top surface of various layers of the present disclosure. [Diagram 2] A cross-sectional SEM image is shown. [Diagram 3] FIG. 2 shows an X-ray diffractogram (intensity on a logarithmic scale to improve visibility of low intensity peaks) of the layer shown in FIG. 1. [Figure 4] 4A and 4B show Raman spectra of the layers shown in FIG. [Diagram 5] 5A and 5B show scanning electron microscope (SEM) images of the top surfaces of various layers of the present disclosure. [Figure 6] 1 shows a scanning electron microscope (SEM) image of the top surface of various layers of the present disclosure. [Figure 7] 1 shows layer thickness growth as a function of duration of the CVD coating process of the present disclosure. [Figure 8] The left image shows a scanning electron microscope (SEM) image of the top surface of the various layers of the present disclosure, and the right image shows a cross-sectional SEM image. [Figure 9] 1 shows the hardness measured by nanoindentation. [Figure 10] The parallel line pattern in the cross-sectional SEM image is shown. [Figure 11] 1 illustrates an example of multiple layers according to the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0034] Coatings comprising cubic polytype silicon carbide (3C-SiC) are endowed with high hardness and strength, good thermal shock resistance and corrosion resistance. Surprisingly, the inventors have discovered that the mechanical and chemical properties of (polycrystalline) silicon carbide coatings can be improved by using an optimized CVD coating method using an aromatic carbon source. The method is capable of producing large SiC deposits and is suitable for large-scale production. Surprisingly, in contrast to the poor results reported in the above-mentioned non-patent document 9, the inventors have succeeded in depositing extremely uniform, {111}-oriented silicon carbide crystals on a large scale on a variety of substrates by optimizing the reaction conditions. Due to the uniformity and very high {111} orientation of the silicon carbide crystals, the coatings are endowed with excellent mechanical and chemical properties.

[0035] In a first aspect, the present disclosure relates to a chemical vapor deposition (CVD) method for preparing a layer comprising silicon carbide crystals, at least a portion of which is formed from a gas mixture containing a silicon source and an aromatic carbon source.

[0036] The C / Si molar ratio of the gas mixture is about 0.85 to about 1.45, more specifically about 0.9 to about 1.3, and especially about 1.0 to about 1.2. By molar ratio is meant the total number of carbon atoms (in moles, or in mol / l) relative to the total number of silicon atoms (in moles, or in mol / l) of the gas mixture present in the reaction chamber. It should be understood that the gas mixture can be premixed or can be individually and independently fed into the reaction chamber.

[0037] In some embodiments, it may be advantageous for the gas to further comprise a halogen source. Suitable halogen sources are well known in the art and may include fluorine, chlorine, and bromine atoms. Specific examples include hydrogen chloride and hydrogen bromide.

[0038] In some embodiments, the silicon source may include a Si-X bond, where X is a hydrogen atom, a hydrocarbyl residue (C 1 ~C 12 Hydrocarbyl residues of 1,2-dichlorophenylsilane, 1,3-dichlorophenylsilane, 1,4-dichlorophenylsilane, 1,5-dichlorophenylsilane, 1,6-dichlorophenylsilane, 1,7-dichlorophenylsilane, 1,8-dichlorophenylsilane, 1,9 ... 1 ~C 4 The alkyl group may comprise a hydrocarbyl residue (such as methyl or ethyl), one or more halogens (such as chlorine), or mixtures thereof.

[0039] In some embodiments, it may be advantageous for at least a portion of the silicon source and at least a portion of the halogen source to be part of the same component of a gas, e.g., where the silicon source includes a Si-X bond, X is a halogen atom.

[0040] In some embodiments, the silicon source is SiCl 4 It can be particularly advantageous to

[0041] In some embodiments, the aromatic carbon source is 6 ~C 30 In some embodiments, the aromatic compound may be benzene, C 1 ~C 6 Alkylbenzene, C 1 ~C 6 Dialkylbenzene, C 1 ~C 6 Trialkylbenzene, C 1 ~C 6 The aromatic compound may be selected from tetraalkylbenzenes, biphenyl derivatives, diphenylmethane derivatives, and naphthalene derivatives, and more specifically, may be a compound selected from benzene, toluene, ethylbenzene, p-xylene, o-xylene, m-xylene, mesitylene, durene, 2-phenylhexane, biphenyl, diphenylmethane, and naphthalene, and in particular may be toluene.

[0042] In some embodiments, the reaction may be carried out under reduced pressure, specifically between about 0 mbar and about 300 mbar, more specifically between about 50 mbar and about 200 mbar, and particularly between about 75 mbar and about 150 mbar. Alternatively, the CVD pressure may be in the range of 10 mbar to 600 mbar, more preferably between 25 mbar and 400 mbar. However, it should be understood that reduced pressure is not necessary, particularly for highly volatile reactants. Thus, in some embodiments, the reaction may be carried out under atmospheric pressure (e.g., about 1 bar).

[0043] In some embodiments, the gas mixture comprises H 2 The gas may further comprise a carrier gas, such as Ar or the like. In some embodiments, the molar ratio of the carrier gas to Si is about 10 to about 40, more specifically about 15 to about 35, and particularly about 20 to about 30. The molar ratio may be determined as described above.

[0044] In some embodiments, the reaction temperature can be about 900° C. to about 1800° C., more particularly about 1000° C. to about 1400° C., and more particularly about 1100° C. to about 1200° C. In some embodiments, the CVD method of the present invention can include thermal CVD. Thermal CVD is distinct from plasma enhanced chemical vapor deposition (PECVD). Thermal CVD typically requires much higher temperatures than PECVD, but does not require a plasma source. As used herein, the term "thermal CVD" refers to CVD at temperatures above 800° C., for example, in the range of 1000° C. to 1400° C.

[0045] In some embodiments it may be particularly advantageous for the method to be thermal CVD, where (all) layers are deposited at a temperature above 800°C, for example in the temperature range of 1000°C to 1400°C.

[0046] In some embodiments, the method may result in a free-standing layer, which may be obtained by depositing a layer on a substrate and subsequently peeling the layer from the substrate.

[0047] In some embodiments the method may comprise depositing said layer on a carbonaceous substrate such as graphite, in particular a wafer carrier comprising graphite, or on a silicon based substrate, in particular a semiconductor substrate comprising silicon such as a wafer, or on a layer comprising a refractory metal carbide such as silicon carbide.

[0048] In a second aspect, the present disclosure relates to a layer comprising silicon carbide crystals, the layer being produced or producible by a method according to the first aspect of the present disclosure.

[0049] The layer is characterized in that, in an SEM image analysis of a cross section of the layer, approximately 20% or less of the area of ​​the cross section has a pattern of parallel lines inclined by more than 15° to the portion of the surface of the layer closest to the respective image. This feature is understood in the context of CVD coating processes to represent highly oriented {111} SiC deposition, meaning that the SiC is preferentially deposited in the {111} orientation, i.e., in a cross section SEM image, the analyzed cross section has lines (growth lines, columnar grains, or twin axes) that appear parallel or substantially parallel to the CVD coated surface. In other words, this feature means that, in an SEM image analysis of a cross section of the layer, the analyzed cross section is characterized in that 80% or more of the area of ​​the cross section has a pattern of parallel lines inclined by less than 15° to the portion of the surface of the layer closest to the respective image. The preparation and analysis of such cross sections is well established in the art. For example, the feature can be determined as follows: ignoring the irregularities of the layer surface, i.e., measuring the angle between a straight line parallel to each portion of the surface and another straight line parallel to the parallel lines of the pattern. In the case of layers that are not flat and have edges, SEM image analysis at the edges is not performed. This can be easily determined by analyzing multiple cross-sectional SEM images. An example of a cross-sectional SEM image is shown in FIG. 10. The cross-section includes different crystalline parts. Each crystalline part has a characteristic pattern of parallel lines. The parallel lines are believed to be caused by twin planes in the silicon carbide crystal. In each crystalline part, the lines are inclined at a certain angle to the layer surface. More specifically, the cross-sectional analysis involves preparing a cross-section cut perpendicular to the surface of the silicon carbide layer, and cutting approximately 1000 μm into the layer surface, including the edges. 2This can be done by obtaining an SEM image of the above cross-sectional area, performing image analysis of the SEM image to determine lines that are substantially parallel to the edge imaged relative to the layer surface, selecting a number of locations on the imaged cross-section (e.g., a random selection of 10 locations distributed across the imaged cross-section), and for each location, performing image analysis of that location to identify the area occupied by parallel lines that are inclined at less than 15° relative to the lines defined as being substantially parallel to the edge imaged relative to the layer surface, and for each location, performing image analysis to determine the area % of that area relative to the total area of ​​each location, and calculating the average area % for all locations to determine the area of ​​the cross-section having a pattern of parallel lines that are inclined at less than 15° relative to a portion of the layer surface.

[0050] In some embodiments, it may be advantageous for SEM image analysis of layer cross sections to show that 18% or less of the area of ​​the cross sections, specifically 16% or less, more specifically 14% or less, and especially 12% or less, has a pattern of parallel lines inclined at more than 15° relative to the portion of the surface of the layer nearest each image.

[0051] The layer comprising silicon carbide crystals may be further characterized as having the following properties:

[0052] In some embodiments, the layer surface comprises silicon carbide crystal apexes in the shape of regular hexagonal pyramids, with less than 10% of the surface being occupied by large regular hexagonal pyramid shaped crystal apexes with a distance from one corner of the apex's regular hexagonal base to the opposite corner of the base being 25 μm or more (surface characteristics); and / or

[0053] The layer comprises silicon carbide crystals, and the Raman spectrum of the layer has two overlapping peaks, the first of which is at 758 cm -1 ~778cm -1 The second peak is at 785 cm -1 ~805cm -1The area ratio calculated by dividing the first area of ​​the first peak by the second area of ​​the second peak is 0.05 or more, specifically 0.06 or more, particularly 0.08 or more, for example 0.12 or more (Raman spectrum characteristic). The area ratio is 1.50 or less, more specifically 1.30 or less, particularly 1.10 or less, for example 0.90 or less, or 0.60 or less. The area ratio range can be determined by these lower and upper limits. 0.05 to 1.50, 0.12 to 1.50, 0.05 to 0.60, and 0.12 to 0.60 are some examples of specific ranges based on specific lower and upper limits.

[0054] The layers of the present disclosure may be described by three properties abbreviated as "surface properties," "cross-sectional properties," and "Raman spectral properties" as mentioned above. However, it should be understood that these properties do not interchangeably define the same coating, i.e., a coating characterized by a "Raman spectral property" does not necessarily also exhibit a "surface property." Similarly, the presence of a "Raman property" or a "surface property" does not necessarily mean that a "cross-sectional property" is also realized. As another example, polishing a surface can eliminate a "surface property" while maintaining a "cross-sectional property."

[0055] From the examples provided below, it will be understood that layers produced by the methods of the present disclosure can have all three properties: "surface properties", "cross-sectional properties", and "Raman spectral properties".

[0056] The present disclosure also relates to layers comprising refractory carbide crystals. Refractory carbides are well known to those skilled in the art of surface coatings in general and chemical vapor deposition (CVD). Refractory carbides include non-carbon carbide components and carbon. For example, in the case of silicon carbide, the non-carbon carbide component is silicon. As will become apparent from the further description below, the present disclosure is not limited to a particular refractory carbide, and silicon carbide is merely an important, but not exclusive, example. Thus, the refractory carbide referred to below is specifically silicon carbide, but does not refer exclusively to silicon carbide.

[0057] As mentioned with respect to the surface characteristics, the layer surface has refractory carbide crystal apexes in the shape of regular hexagonal pyramids. The term "regular hexagonal pyramid" has its usual meaning in the art and refers to a pyramid with a regular hexagonal base, i.e., a pyramid with a hexagonal base with all six angles equal in size and all six sides of the same length. The apexes of the refractory carbide crystals are the portions of the crystals visible in the SEM image of the surface. The total height of the crystals is generally much higher than the height of the pyramid apex exposed at the surface. Many crystals are oriented nearly or completely perpendicular to the surface, and the apexes of the crystals visible in the SEM image match very well with the shape of the hexagonal pyramids used to describe the "surface characteristics" of the layers of the present disclosure. In some embodiments, the shape of the hexagonal pyramids can be faceted.

[0058] As further described with respect to the surface characteristics, less than 10% of the surface is occupied by crystal apices in the shape of large hexagonal pyramids, with the distance from one corner of the base of the hexagonal apices to the diagonal of the base being 25 μm or more. The percentage of the surface occupied by such large crystal apices can be determined quite easily by analyzing multiple surface SEM images. Each portion of the surface covered by a single crystal apice that completely occupies a hexagonal base, with the distance from one corner of the base to the diagonal of the base being 25 μm or more, constitutes a particular surface portion occupied by the large crystal apices. Other portions of the surface are not considered to be surface occupied by the large crystal apices.

[0059] When determining whether a particular percentage of the surface is occupied by large crystal tips, surface irregularities (such as those caused by the inclination of the crystal tips of pyramids) are not taken into account. The surface is assumed to be perfectly flat when determining the surface percentage. Thus, a top-view SEM image can be analyzed to determine whether a given percentage fits the particular layer under consideration.

[0060] In this application, the term "hexagonal" does not refer to the stacking of atomic lattices within a crystal (hexagonal crystal). In this application, the term "hexagonal" refers to the external shape of a crystal or a crystal part as seen in an SEM image, and does not refer to a type of crystal.

[0061] In some embodiments, less than 9% of the surface is occupied by large regular hexagonal pyramidal shaped crystal apices, the distance from one corner of the base of the apex regular hexagon to the opposite corner of the base being 25 μm or more, more particularly less than 8%, in particular less than 7%, for example less than 6%.

[0062] The Raman spectral characteristics define the layers of the present disclosure by two overlapping peaks in the Raman spectrum of the layer. In this application, the Raman spectrum is obtained by illuminating the exposed surface of the layer perpendicularly with an Ar laser operating at a wavelength of 532 nm and a power of 10 mW. As explained below, the area of ​​both peaks is approximately 730 cm. -1 ~About 840cm -1 The peaks can be derived by fitting the intensities in the range of 763 cm to two lines of approximate shape (for example, a linear combination of a Gaussian function and a Lorentzian function). -1 ~774cm -1 , more specifically 765 cm -1 ~772cm -1 , for example 767cm -1 ~770cm -1 and the second peak is typically at 790 cm -1 ~801cm -1 , more specifically 792 cm -1 ~799cm -1 , for example 794cm -1 ~797cm -1 The maximum strength is in the range of

[0063] In some embodiments, 10% or more of the surface is covered by the apexes of regular hexagonal pyramids, specifically 15% or more, more specifically 20% or more, especially 25% or more. This includes all the apexes of regular hexagonal pyramids, regardless of the size of the apexes or the bases of the regular hexagonal pyramids. This represents high crystal quality and a high degree of preferred orientation, improving hardness. Without being bound by theory, it is believed that the etch resistance is improved. The increase in this portion is an indication of the hexagonal base crystals approaching a honeycomb arrangement. Without being bound by theory, it is believed that the regular arrangement of such crystals reduces the number of deep pitches, which in turn reduces the tendency to corrode.

[0064] In some embodiments, the layers of the present disclosure have a surface with a mean linear intercept surface grain size (as defined in ISO13382-1:2012 (EN)) in the range of 0.2 μm to 25 μm, typically 0.4 μm to 20 μm, e.g., 0.5 μm to 15 μm. Without being bound by theory, it is believed that this provides useful etchability. The above grain size range represents a relatively large crystal size. Many smaller crystals are quickly etched due to long grain boundaries, and a small number of large crystals promote large, possibly wedge-shaped gaps that promote the penetration of significant amounts of etching gas deep into the layer. In some embodiments, the layers of the present disclosure have a surface with a mean linear intercept surface grain size (as defined in ISO13382-1:2012 (EN)) in the range of 1 μm to 20 μm, more specifically 1.2 μm to 15 μm, especially 2 to 10 μm.

[0065] In some embodiments, the refractory carbide is selected from silicon carbide, tantalum carbide, niobium carbide, hafnium carbide, tungsten carbide, boron carbide, tantalum niobium carbide, tantalum hafnium carbide, titanium carbide, and niobium hafnium carbide, in particular silicon carbide, tantalum carbide, niobium carbide, titanium carbide, and hafnium carbide. As mentioned above, it may be particularly advantageous for the refractory carbide to be silicon carbide. The refractory carbide crystal is in particular a silicon carbide crystal.

[0066] As mentioned above, apart from the specific context, the term "refractory carbide" as used herein refers specifically to "silicon carbide." Although specific effects are shown herein with respect to silicon carbide, it is reasonable to assume that the same or similar effects will be observed with other refractory carbides, since the growth of various refractory carbides in CVD follows the same or similar physical principles, as shown in the examples below.

[0067] In some embodiments, the maximum peak intensity I in an X-ray diffractogram of the layer detected with CuKα radiation having a wavelength of 1.5406 Å 220 is the maximum peak intensity I 110 of the surface, specifically 8% or less, more specifically 7% or less, even more specifically 6% or less, especially 5% or less. This results in high crystal quality and strong crystal orientation. The (111) plane is the closest packed plane in the cubic crystal system. The orientation of this plane parallel to the surface provides high mechanical stability and improved corrosion resistance. Without being bound by theory, the inventors believe that this increases the number of crystals that fit closely to neighboring crystals. As a result, the probability of deep pitch is low and corrosion may be slower.

[0068] In some embodiments, a layer according to the present disclosure may have a distribution of silicon carbide crystal orientations such that the orientation quality Q, calculated from the maximum peak intensity of an X-ray diffractogram detected with CuKα radiation at a wavelength of 1.5406 Å according to the following formula, is 0.60 or more, specifically 0.80 or more, more specifically 0.90 or more, even more specifically 0.95 or more, especially 0.99 or more, which is believed to further contribute to the hardness and corrosion resistance of the layer: Q=(I 111 +I 222 +I 333 / 511 ) / (I 111 +I 200 +I 220 +I 311 +I 222 +I 400 +I 331 +I 420 +I 333 / 511 +I 422 ) During the ceremony, I 111 is the maximum intensity at 2θ in the range of 34.6° to 36.6°, I 200 is the maximum intensity at 2θ in the range of 40.4° to 42.4°, I 220 is the maximum intensity at 2θ in the range of 59.0° to 61.0°, I 311 is the maximum intensity at 2θ in the range of 70.8° to 72.8°, I 222 is the maximum intensity at 2θ in the range of 74.5° to 76.5°, I 400 is the maximum intensity at 2θ in the range of 89.0° to 91.0°, I 331 is the maximum intensity at 2θ in the range of 99.8° to 101.8°, I 420 is the maximum intensity at 2θ in the range of 103.4° to 105.4°, I 333 / 511 is the maximum intensity at 2θ in the range of 132.4° to 134.4°, I 422 is the maximum intensity at 2θ in the range of 119.0° to 121.0°.

[0069] In some embodiments, I 200 , I 220 , I 311 , I 400 , I 331 , I 420 , I 422 Each intensity is a corresponding reference intensity I predicted for a randomly distributed silicon carbide crystal orientation. 200 R,I 220 R,I 311 R,I 400 R,I 331 R,I 420 R,I 422 R is 80% or less, specifically 60% or less, more specifically 40% or less, and particularly 30% or less.

[0070] In some embodiments, the layer has a peak intensity I having a full width at half maximum (FWHM) value of less than about 0.4°, more particularly less than about 0.3°, and especially less than 0.2° (at 2θ with CuKα radiation of wavelength 1.5406 Å). 111 This characteristic is indicative of the relatively large crystals that may be obtained by the thermal CVD method according to the present disclosure, which promotes the growth of large crystals.

[0071] In some embodiments, the layers of the present disclosure have a peak intensity I having a full width at half maximum (FWHM) value of less than about 0.4°, more particularly less than about 0.3°, and especially less than 0.2° (at 2θ with CuKα radiation of wavelength 1.5406 Å). 111 and a surface having a mean linear intercept surface grain size (as defined in ISO 13382-1:2012 (EN)) in the range of 1 μm to 20 μm, more particularly 1.2 μm to 15 μm, in particular 2 to 10 μm.

[0072] In some embodiments, the layer of the present disclosure has a hardness of 34.0 GPa or more, preferably 34.5 GPa or more, for example 35.0 GPa or more. The hardness is measured orthogonally to the layer surface by nanoindentation after polishing the layer surface. The polished surface on which the hardness is measured is the surface formed by the edges of the crystals that grow gradually during the CVD method of the present disclosure. Polishing is performed such that the tops of the crystals are flat. The unusually high hardness improves the life of parts coated with the layer of the present disclosure, since it reduces mechanical damage during handling and use of the parts.

[0073] In some embodiments, the surface hardness of the layer is at least 0.5%, particularly at least 1%, more particularly at least 1.5%, especially at least 2.0% higher than the cross-sectional hardness of the layer. The cross-sectional hardness is measured by nanoindentation after polishing a cross-section of the layer. The cross-section is perpendicular to one or both surfaces of the layer. Without being bound by theory, it is believed that the extraordinary hardness from the top is due to the highly consistent orientation.

[0074] A layer can be a layer on the surface of a component of a device, or a free-standing layer. A free-standing layer does not include a substrate. Neither of the two major surfaces of a typical free-standing layer is attached to a substrate.

[0075] The present disclosure further relates to a device for high temperature applications, the device comprising a layer of the present disclosure on a surface of a material of the device, the high temperature typically referring to temperatures in the range of 200°C to 4000°C, particularly 300°C to 3000°C, and especially 400°C to 2500°C.

[0076] The material of the device is not particularly limited. All materials suitable for the high temperatures of the above high temperature applications are suitable as the material of the device. In some embodiments, the material of the device includes graphite, silicon element, and heat-resistant refractory materials, such as silicon carbide. The material of the device can be, for example, a graphite material, a carbon fiber reinforced material, or silicon element. The silicon element can be, in particular, in the form of a wafer, such as that used in the semiconductor industry. The material can have the shape of a support for semiconductor applications. As is well known in the art, supports for semiconductor applications often have the shape of a disk with one or more recesses for placing a semiconductor substrate, such as a silicon-based wafer, to be processed on the support, for example, in epitaxy reactors, MOCVD (metal organic chemical vapor deposition) reactors, where such supports are typically used to grow layers on wafers, and in plasma etching reactors, such as focus rings and RTP (rapid thermal processing) reactors (i.e., RTP rings). However, the device can also be a component of other high temperature reactors or high temperature furnaces. The component may be, for example, a heater, a charging rack or charging rack parts (eg, strips), a baffle, or other CVD chamber components other than the wafer carrier, such as lift pins, ceiling, inlets, outlets, etc. of the CVD chamber.

[0077] The layer may be a single layer of a multilayer. The multilayer comprises at least one other layer. The one or more other layers may each be, for example, another refractory carbide layer or a carbon-based layer. The multilayer may be a free-standing multilayer. The multilayer may also be a coating deposited on a surface of the device.

[0078] In some embodiments, the layer may be multi-layered, comprising one or more layers according to the present disclosure and one or more additional silicon carbide layers.

[0079] The thickness of the layer is generally 0.5 μm or more. In some embodiments, when the layer is a layer of a device (e.g., a device of the present disclosure), the thickness of the layer is in the range of 1 μm to 1 mm. This ensures reliable protection of the material coated with the layer at reasonable deposition times and therefore reasonable costs. In some embodiments, when the layer is a free-standing layer, i.e., a free-standing layer of the present disclosure, the thickness of the layer is in the range of 100 μm to 100 mm.

[0080] In alternative embodiments, the layer thickness may be greater than or equal to about 0.5 μm, more particularly greater than or equal to about 1 μm, and especially greater than or equal to about 10 μm. In some embodiments, it may be particularly advantageous for the layer thickness to be greater than or equal to 50 μm.

[0081] The layer comprising heat-resistant carbide crystals to which the present disclosure further relates, preferably the layer of the present disclosure, is a free-standing layer, and the average roughness Ra (defined by ISO 4287) of one surface of the layer is: in the range of 0.01 nm to 100 nm, specifically 0.02 nm to 50 nm, in particular 0.04 nm to 25 nm, for example 0.08 nm to 15 nm (nanoscale roughness); in the range of 0.1 nm to 100 nm, specifically 0.2 nm to 50 nm, in particular 0.4 nm to 25 nm, for example 0.8 nm to 15 nm (nanoscale roughness); or It is in the range of 100 nm to 10 μm, specifically 200 nm to 8 μm, in particular 300 nm to 6 μm, for example 400 nm to 5 μm (microscale roughness).

[0082] Nanoscale roughness is measured by atomic force microscopy. Microscale roughness is measured by profilometry. Both measurement techniques are well known in the art.

[0083] The layer of the present disclosure, in which one surface of the layer has nanoscale roughness, can be formed by using a single crystal substrate, particularly single crystal silicon, e.g., a silicon wafer, in the method of the present disclosure, depositing the layer on the single crystal substrate, and removing the substrate from the layer. Removing the substrate from the layer can include thermally removing the substrate from the layer, e.g., melting the silicon. The inventors have discovered that the nanoscale roughness of the single crystal silicon surface is carried over to the surface of the layer.

[0084] The layers of the present disclosure having microscale roughness on one surface of the layer can be formed by using a graphite substrate, particularly an isostatic graphite substrate, in the methods of the present disclosure, depositing the layer on the graphite substrate, and removing the substrate from the layer. Removal of the substrate from the layer can include mechanical and / or oxidative degradation of the graphite substrate. The inventors have discovered that the microscale roughness of the graphite surface, which is due to the graphite grains, is carried over to the surface of the layer.

[0085] The nanoscale or microscale roughness is obtained at the surface of the layer that is in contact with the substrate after deposition of the layer: this surface of the free-standing layer matches the roughness of the substrate, while the opposite surface may have a roughness of 0.01 nm or more, obtained by the above-mentioned "surface characteristics" or by standard polishing (e.g. CMP).

[0086] A preferred free-standing layer of the present disclosure has one surface having a nanoscale or microscale roughness as defined herein, preferably a nanoscale roughness as defined herein, and further has a "surface characteristic" as defined herein, and / or a "cross-sectional characteristic" as defined herein, and / or a "Raman spectral characteristic" as defined herein, on a surface opposite the surface having the nanoscale roughness.

[0087] Further, the present disclosure relates to the use of the disclosed layers, devices, wafer carriers, and layers, devices, and wafer carriers made according to the disclosed methods to support semiconductors. With respect to free-standing layers, one specific embodiment of such a free-standing layer is a wafer for the deposition of semiconductors.

[0088] Also in accordance with the above disclosure, the present disclosure provides in a third aspect a layer comprising silicon carbide crystals having a distribution of silicon carbide crystal orientations with an orientation quality Q of about 0.90 or more, specifically about 0.95 or more, more specifically about 0.97 or more, particularly about 0.99 or more, the orientation quality Q being calculated from the maximum peak intensity of an X-ray diffractogram detected with CuKα radiation having a wavelength of 1.5406 Å according to the following formula: Q=(I 111 +I 222 +I 333 / 511 ) / (I 111 +I 200 +I 220 +I 311 +I 222 +I 400 +I 331 +I 420 +I 333 / 511 +I 422 ) During the ceremony, I 111 is the maximum intensity at 2θ in the range of 34.6° to 36.6°, I 200 is the maximum intensity at 2θ in the range of 40.4° to 42.4°, I 220 is the maximum intensity at 2θ in the range of 59.0° to 61.0°, I 311 is the maximum intensity at 2θ in the range of 70.8° to 72.8°, I 222 is the maximum intensity at 2θ in the range of 74.5° to 76.5°, I 400 is the maximum intensity at 2θ in the range of 89.0° to 91.0°, I 331 is the maximum intensity at 2θ in the range of 99.8° to 101.8°, I420 is the maximum intensity at 2θ in the range of 103.4° to 105.4°, I 333 / 511 is the maximum intensity at 2θ in the range of 132.4° to 134.4°, I 422 is the maximum intensity at 2θ in the range of 119.0° to 121.0°.

[0089] In some embodiments, the layer may be provided with the characteristics described with respect to the second aspect of the present disclosure.

[0090] In a fourth aspect, the present disclosure relates to a device, in particular a wafer carrier, for high temperature applications, comprising a layer according to the second or third aspect of the present disclosure, the layer being provided on a surface of the device.

[0091] In a fifth aspect, the present disclosure relates to the use of a layer according to the second or third aspect of the present disclosure for supporting a semiconductor.

[0092] In the following the present disclosure will be explained in more detail by means of non-limiting figures and examples.

[0093] Example 1 - Growth on graphite at various temperatures (sample 1 and sample 2) Isostatic graphite substrates were coated with silicon carbide in a CVD chamber. The CVD reactor consisted of an inductively heated SiC-coated graphite susceptor insulated with graphite felt (MFA insulation from SGL Carbon Corp.) and placed inside a quartz tube. The carrier gas was H 2 The inlet side of the reactor was connected to a gas supply system for supplying the precursors silicon tetrachloride and toluene, and the outlet side of the reactor was connected to a vacuum pump and a scrubbing system via a throttle valve.

[0094] Two graphite substrates were each coated with one layer comprising silicon carbide crystals according to the present disclosure. The layers were formed under the CVD growth conditions summarized in Table 1.

[0095] [Table 1]

[0096] The surfaces of the coated samples were covered with hexagonal, well-faceted SiC crystals. Regular hexagonal pyramidal shaped silicon carbide crystal apices can be seen in the layers of both Sample 1 (left) and Sample 2 (right) in Fig. 1. As the crystal apices are rather small, it can be seen at a glance that less than 10% of the surface is occupied by large regular hexagonal pyramidal shaped crystal apices with a distance from one corner of the base of the hexagon of the apices to the opposite corner of the base of the base of more than 25 μm. This morphology is present in most of the surface and is uniform, at least over the part examined by SEM. The dark spots in the crystal centers are artifacts due to charging effects and are not present when the samples are sputter-coated with a conductive metal before examination by SEM. The mean linear intercept surface grain size (defined in ISO13383-1:2012 (EN)) of Sample 1 prepared at 1100 °C was 1.2 μm. The mean linear intercept surface grain size of sample 2 prepared at 1200°C was 2.6 μm.

[0097] Cross-sectional SEM images reveal a columnar structure of grains growing from the graphite surface (Fig. 2). The lines parallel to the surface are due to twin planes within the SiC crystal. These twin planes are likely to be parallel to the (111) crystal plane.

[0098] Figure 3 shows the X-ray diffractograms of Sample 1 (top) and Sample 2 (bottom). The intensities are plotted on a logarithmic scale to improve the visibility of the low intensity peaks. The peaks indicated by squares are due to β-SiC, and the peaks indicated by circles are due to graphite. The X-ray diffractograms (3) of Samples 1 and 2 show only three strong peaks. These peaks are located at 2θ values ​​of 35.6°, 75.2°, and almost 133°, as shown on the horizontal axis, and are assigned to the (111), (222), and (333) / (511) planes of the β-SiC crystal.

[0099] It is noted that both the (333) and (511) planes of β-SiC give rise to signals with 2θ ranging from 132.4° to 134.4° and are indistinguishable. Therefore, this signal is denoted as (333) / (511). The fact that only the (111) and (222) signals are visible with high intensity leads to the conclusion that the third peak is mainly caused by the (333) plane. All three planes are parallel and belong to the same family of crystallographic planes.

[0100] The (111) signal is the strongest signal, with the (222) and (333) / (511) signals being less than 4% of the (111) signal (Table 2). The strongest β-SiC XRD signals not caused by planes parallel to the (111) plane are the (220) signal (0.13%) for sample 1 and the (311) and (420) signals (0.11%) for sample 2. The extremely low signal intensities of planes not parallel to (111) indicate a strong preferred orientation of the crystals of the layers of the present disclosure. The intensity of the (111) orientation can be quantified by the orientation quality Q of the signal of the (111)+(222)+(333) / (511) plane series relative to the total XRD signal intensity of all signals according to the following formula: Q=(I 111 +I 222 +I 333 / 511 ) / (I 111 +I 200 +I 220 +I 311 +I 222 +I 400 +I 331 +I420 +I 333 / 511 +I 422 )

[0101] The orientation quality Q is 1 if only (111), (222) and (333) / (511) signals are detected, i.e. all measured crystals are perfectly oriented with their (111) planes parallel to the substrate surface. The orientation quality Q is 0 if no (111) series signals are detected, i.e. none of the measured crystals are oriented with their (111) planes parallel to the substrate surface. The expected orientation quality Q for randomly oriented powder is 0.5116 due to expected signal intensity variations.

[0102] [Table 2]

[0103] Random powder values ​​are taken from powder diffraction file (PDF card) #00‐029‐1129.

[0104] All intensities reported in this application are maximum intensities, that is, the intensities derived from the highest points of the corresponding peaks in the X-ray diffractogram.

[0105] Samples 1 and 2 were further characterized by Raman spectroscopy (Figures 4A and 4B). The numbers on the horizontal axis are wavenumbers (cm -1 The main features of the spectrum are the very strong TO and LO signals of β-SiC (786 cm -1 and 963cm -1 ) and their secondary peaks (1514 cm -1 and 1703 cm -1 ) From Figure 4B, it is approximately 786 cm -1 It can be seen that the signal with a maximum at 1612 cm is due to two overlapping peaks. -1The minor peaks around 196 cm can be attributed to graphitic carbon. -1 and 462cm -1 The LA and TA signals can be seen, indicating a small particle size.

[0106] Figure 4B shows the 730 cm -1 ~840cm -1 The Raman spectra of layers of sample 1 (left) and sample 2 (right) with two overlapping peaks in the range of 768 cm 2 . For both samples, the overlapping peaks were fitted with a pseudo-Voigt curve (a linear combination of a Gaussian and a Lorentzian function). The fitting was done without any special background processing. This resulted in the first of the two peaks being located at 768 cm 2 . -1 The maximum intensity is at 795 cm and the second peak is at 795 cm. -1 ~796cm -1 It was found that the peaks had the maximum intensity at 100 nm and 150 nm at 100 nm. Further details are given in Table 3. The area ratio calculated by dividing the first area of ​​the first peak by the second area of ​​the second peak was 0.33 for sample 1 and 0.30 for sample 2.

[0107] [Table 3]

[0108] Example 2 - Growth on graphite with various C / Si ratios Several deposition experiments were performed to investigate the effect of carbon precursor concentration on the coating and the resulting C / Si gas phase molar ratio. The C / Si was varied by varying the toluene flow while keeping other parameters constant (in Table 4, sample 2 is from Example 1 above).

[0109] [Table 4]

[0110] 1A and 5B show SEM top-view images of graphite substrates coated with layers formed under various conditions in Table 4. Sample 2 is shown in the right panel of FIG. 5A. Sample 4 is shown in the left panel of FIG. 5B. The left panel of FIG. 5A (Comparative Sample 3) and the right panel of FIG. 5B (Comparative Sample 5) show SEM top-view images of other layers made under extreme conditions of molar excess of carbon and molar excess of silicon, respectively. Only Samples 2 and 4 show the characteristic silicon carbide crystal tops of the present disclosure. On the other hand, coatings with molar excess of either carbon or silicon produced different surface morphologies and essentially did not have the refractory carbide crystal tops with regular hexagonal pyramid shapes.

[0111] The intensities of the XRD peaks are summarized in Table 5. The XRD peak intensities of Comparative Sample 3 are much closer to randomly oriented powder than Sample 2 and Sample 4, indicating the absence of a strong preferred crystal orientation in the layer of Sample 3. Samples 2 and 4 have the (111) peak as the most intense peak, followed by the (222) and (333) / (511) peaks, indicating a strong (111) preferred orientation of the coating. The most intense peaks from other series of planes are the (311) and (420) peaks at 0.11% for Sample 2 and the (311) peak at 0.80% for Sample 4. In Comparative Sample 5, the (220) peak is the most intense, followed by the (111) peak at 17.58%, indicating a strong (220) orientation of the coating. While the formation of the layers of the present disclosure is not promoted at the extreme C / Si molar ratios, the layers of the present disclosure appear to form easily within the range between these two extreme C / Si molar ratios. The range includes a C / Si molar ratio of 1.0 to 1.2.

[0112] [Table 5]

[0113] Example 3 - Growth on graphite with varying deposition times The thickness of the layer of the present disclosure can be adjusted by changing the deposition time. In addition to sample 2 of Example 1 (deposition time 30 minutes), sample 6 was accompanied by deposition shortened to only 5 minutes, and sample 7 was accompanied by deposition extended to 60 minutes (Table 6). The remaining process conditions remained unchanged.

[0114] [Table 6]

[0115] figure 7 shows the average layer thickness (vertical axis, in μm) as a function of deposition time (horizontal axis, in minutes) for samples 2, 6 and 7. .sa The surfaces of Samples 6 and 7 contain hexagonal pyramidal crystal tops. nothing. Grain size and coating thickness (Fig. 7 ) increase with increasing deposition time from Sample 6 to Sample 2 and from Sample 2 to Sample 7. This demonstrates that the preferred orientation does not change as the coating grows thicker and is not a surface effect of the substrate. In fact, the XRD data in Table 7 demonstrate that as the thickness increases, the crystals become more oriented in the (111) direction, indicating that the preferred orientation coating is a result of the coating process itself.

[0116] [Table 7]

[0117] Example 4 - Growth on silicon wafers The CVD method demonstrated in this application can produce highly (111)-oriented β-SiC coatings not only on polycrystalline isotropic substrates (such as isostatic graphite) but also on single crystal substrates (such as silicon wafers). (hkl) orientation in this disclosure means that the (hkl) planes (and their parallel crystal planes) are mainly oriented parallel to the layer surface. If the two crystal structures of the substrate and the layer are sufficiently similar (epitaxial growth), the single crystal substrate can influence the growth so that the growing layer follows a crystal orientation just like that of the substrate. A piece of (100)-oriented silicon wafer was coated with β-SiC (sample 8) under similar conditions as sample 2 in Example 1. Again, the surface coating is composed of crystals exhibiting a hexagonal pattern (Figure 8). The cross section reveals a columnar and well-ordered growth of highly oriented crystals. XRD also shows that the coating is highly (111)-oriented with a Q of 0.9993.

[0118] [Table 8]

[0119] Example 5 - Nanoindentation measurements Hardness was measured by nanoindentation on polished surfaces, with coatings at least 100 μm thick to avoid substrate influence on hardness measurements. Nanoindentation measurements were performed on a variety of refractory carbide layers of the present disclosure with different crystal orientations (quantified by the ratio Q). For all samples, measurements were performed on the polished cross-sections, and for coatings with thicknesses greater than 100 μm, measurements were also performed on the polished top surface.

[0120] In Fig. 9 the results of nanoindentation measurements (vertical axis, in GPa) are plotted against the orientation quality Q (horizontal axis) of the investigated samples. The open squares show the results of nanoindentation measurements on the polished top surface. The filled circles show the results of nanoindentation measurements on the polished cross section.

[0121] Surprisingly, it has been found that in the refractory carbide layer, the SiC crystals have one or more of the "surface characteristics", "cross-sectional characteristics" and "Raman spectrum characteristics" described herein, and also have very high hardness when measured from the top surface. Even more surprisingly, the hardness of the top surface measurement increased with increasing Q, from about 35 GPa to about 38 GPa. The hardness of the cross-sectional measurements followed the opposite trend, decreasing with increasing Q. This opposing trend is believed to be the result of a strong preferred crystal orientation. When measuring hardness on a cross-section, the force is actually applied at an angle of 90° to the preferred orientation plane. If the more resistant (111) plane is oriented parallel to the substrate, the hardness measured on the cross-section will decrease. This idea is further supported by the atomic density. The (111) plane of β-SiC has the highest atomic density and supports an unusually high hardness perpendicular to that plane, but the "planes" perpendicular to the (111) plane have a significantly lower atomic density. The decrease in atomic density in this case is believed to be associated with a decrease in hardness. Furthermore, the high atomic density parallel to the surface is believed to be most resistant to the etchant.

[0122] FIG. 10 shows an SEM image of a cross-section of a layer of Sample 2. The horizontal line at the top of FIG. 10 is parallel to the layer surface. The dashed line is aligned with the parallel line of the most strongly tilted grains in the cross-section. The angle between the horizontal line and the dashed line is 12°. In this cross-section, nearly 0% of the area of ​​the cross-section has a pattern of parallel lines that are tilted at more than 15° to the layer surface. To determine the exact percentage of the area of ​​the cross-section that is tilted at more than a given angle to the layer surface, one skilled in the art would analyze multiple SEM images.

[0123] Example 6 - Growth of multilayer structures with highly (111) oriented SiC The layers of this disclosure can also be part of a multi-layer structure. In this example, a six-layer coating system with three highly (111) oriented layers and three non-(111) oriented layers was deposited on an isostatic graphite substrate. These six layers were produced by switching the hydrocarbon source and changing the C / Si ratio during the process.

[0124] [Table 9]

[0125] As can be seen in FIG. 11, the orientation of the layers is visible by a pattern of lines parallel to the surface, which can be changed during the deposition process. The lines are easily visible in the exemplary enlarged view shown in the right diagram of FIG. 11. In the coating of Example 6, the second, fourth and sixth layers (counting from the substrate) are layers of the present disclosure, while the first, third and fifth layers are not oriented in the (111) direction. Such a multilayer structure can reduce the risk of forming etching pinholes in the cleaning process and can also reduce damage induced by chipping of the coating from the substrate under high mechanical loads.

[0126] The present application further relates to the following embodiments:

[0127] EMBODIMENT 1 A layer comprising heat-resistant carbide crystals, The surface of the layer comprises refractory carbide crystal apexes in the shape of regular hexagonal pyramids, with less than 10% of the surface being occupied by large regular hexagonal pyramid-shaped crystal apexes having a distance from one corner of the base of the regular hexagon of the apex to the opposite corner of the base of the base of the regular hexagon of the apex being 25 μm or more; and / or and / or, upon SEM image analysis of a cross-section of the layer, less than 20% of the area of ​​the cross-section has a pattern of parallel lines that are inclined by more than 15° relative to the portion of the surface of the layer closest to the respective image. The heat-resistant carbide crystal is a silicon carbide crystal, and the Raman spectrum of the layer has two overlapping peaks, the first of the two peaks being at 758 cm -1 ~778cm -1 The maximum intensity is in the range of 785 cm -1 ~805cm -1and an area ratio calculated by dividing a first area of ​​a first peak by a second area of ​​a second peak is 0.05 or greater.

[0128] EMBODIMENT 2 2. The layer of embodiment 1, wherein 10% or more of the surface is covered by the apexes of regular hexagonal pyramid shapes.

[0129] EMBODIMENT 3 2. The layer of embodiment 1, wherein the surface has a mean linear intercept surface grain size in the range of 0.2 μm to 25 μm.

[0130] EMBODIMENT 4 2. The layer of embodiment 1, wherein the refractory carbide crystals are silicon carbide crystals.

[0131] EMBODIMENT 5 X-ray diffractogram of the layer detected with CuKα radiation at a wavelength of 1.5406 Å 220 The maximum peak intensity is I 111 2. The layer of embodiment 1, wherein the intensity is 10% or less of the maximum peak intensity.

[0132] EMBODIMENT 6 The distribution of orientation of the silicon carbide crystals is such that the orientation quality Q is 0.60 or more, the orientation quality Q being calculated from the maximum peak intensity of an X-ray diffractogram detected with CuKα radiation at a wavelength of 1.5406 Å according to the following formula: Q=(I 111 +I 222 +I 333 / 511 ) / (I 111 +I 200 +I 220 +I 311 +I 222 +I 400 +I 331 +I 420 +I 333 / 511 +I 422 ) During the ceremony, I 111is the maximum intensity at 2θ in the range of 34.6° to 36.6°, I 200 is the maximum intensity at 2θ in the range of 40.4° to 42.4°, I 220 is the maximum intensity at 2θ in the range of 59.0° to 61.0°, I 311 is the maximum intensity at 2θ in the range of 70.8° to 72.8°, I 222 is the maximum intensity at 2θ in the range of 74.5° to 76.5°, I 400 is the maximum intensity at 2θ in the range of 89.0° to 91.0°, I 331 is the maximum intensity at 2θ in the range of 99.8° to 101.8°, I 420 is the maximum intensity at 2θ in the range of 103.4° to 105.4°, I 333 / 511 is the maximum intensity at 2θ in the range of 132.4° to 134.4°, I 422 is a maximum intensity at 2θ in the range of 119.0° to 121.0°.

[0133] EMBODIMENT 7 I 200 , I 220 , I 311 , I 400 , I 331 , I 420 , I 422 Each intensity in is the corresponding reference intensity I predicted for a randomly distributed silicon carbide crystal orientation. 200 R,I 220 R,I 311 R,I 400 R,I 331 R,I 420 R,I 422 7. The layer of embodiment 6, wherein R is 80% or less.

[0134] EMBODIMENT 8 2. The layer of embodiment 1, wherein the surface hardness of the layer is at least 0.5% greater than the cross-sectional hardness of the layer.

[0135] EMBODIMENT 9 A device for high temperature applications comprising a layer of any of the preceding embodiments on a material surface of said device.

[0136] EMBODIMENT 10 10. The device of embodiment 9, wherein the material of the device comprises graphite, elemental silicon, or silicon carbide.

[0137] EMBODIMENT 11 A heat resistant carbide coated wafer carrier comprising or made of the layer of any of the preceding embodiments.

[0138] EMBODIMENT 12 A CVD method for preparing the layer according to embodiment 1, the device according to embodiment 9, or the wafer carrier according to embodiment 11, comprising: The method wherein at least a portion of the layer is formed from a gas containing a silicon source and an aromatic carbon source.

[0139] EMBODIMENT 13 A layer comprising heat-resistant carbide crystals, preferably as described in embodiment 1, wherein the layer is a free-standing layer and the roughness of one surface of the layer is in the range of 0.01 nm to 100 nm, or in the range of 100 nm to 10 μm.

[0140] EMBODIMENT 14 Use of a layer according to any one of embodiments 1 to 8, 13, a device according to embodiment 9 or 10, a heat-resistant carbide-coated wafer carrier according to embodiment 11, or a layer, device or wafer carrier made by the method according to embodiment 12, for supporting a semiconductor.

Claims

1. 1. A chemical vapor deposition (CVD) method for preparing a layer of silicon carbide crystals, wherein at least a portion of said layer is formed from a gas mixture containing a silicon source and an aromatic carbon source, said gas mixture having a C / Si molar ratio of 0.85 to 1.

45.

2. The aromatic carbon source is 6 ~C 30 2. The chemical vapor deposition method of claim 1 , wherein the aromatic compound is

3. The chemical vapor deposition method according to claim 1 or 2, wherein the reaction temperature is from 900°C to 1800°C.

4. The reaction is carried out under reduced pressure, and / or The chemical vapor deposition method of claim 1 , wherein the gas mixture further comprises an inert carrier gas.

5. the chemical vapor deposition process produces a free-standing layer; or 5. The chemical vapor deposition method according to claim 1, wherein the layer is deposited on a carbonaceous substrate, on a silicon-based substrate, or on a layer of refractory metal carbide.

6. 1. A layer comprising silicon carbide crystals, wherein upon SEM image analysis of a cross-section of the layer, 20% or less of the cross-sectional area has parallel growth lines of the silicon carbide crystals that are inclined at an angle of more than 15° relative to a surface of the layer.

7. The surface of the layer comprises silicon carbide crystal apexes in the shape of regular hexagonal pyramids, with less than 10% of the surface being occupied by large regular hexagonal pyramid apexes having a distance from one corner of the base of the regular hexagon to the opposite corner of the regular hexagon being 25 μm or more; and / or The layer is characterized by a Raman spectrum having two overlapping peaks, the first of the two peaks being at 758 cm -1 ~778cm -1 and a second peak at 785 cm -1 ~805cm -1and an area ratio calculated by dividing a first area of ​​the first peak by a second area of ​​the second peak is 0.05 or greater.

8. The layer of claim 7 , wherein 10% or more of said surface comprises said regular hexagonal pyramidal shaped silicon carbide crystal tops.

9. The distribution of silicon carbide crystal orientation is such that the orientation quality Q is 0.90 or more; The orientation quality Q is calculated from the maximum peak intensity of an X-ray diffractogram detected with CuKα radiation at a wavelength of 1.5406 Å according to the following formula: Q = (I 111 +I 222 +I 333/511 ) / (I 111 +I 200 +I 220 +I 311 +I 222 +I 400 +I 331 +I 420 +I 333/511 +I 422 ) I 111 is the maximum intensity at 2θ in the range 34.6° to 36.6°, I 200 is the maximum intensity at 2θ in the range of 40.4° to 42.4°, I 220 is the maximum intensity at 2θ in the range of 59.0° to 61.0°, I 311 is the maximum intensity at 2θ in the range of 70.8° to 72.8°, I 222 is the maximum intensity at 2θ in the range of 74.5° to 76.5°, I 400 is the maximum intensity at 2θ in the range of 89.0° to 91.0°, I 331 is the maximum intensity at 2θ in the range of 99.8° to 101.8°, I 420 is the maximum intensity at 2θ in the range of 103.4° to 105.4°, I 333/511 is the maximum intensity at 2θ in the range of 132.4° to 134.4°, I 422 A layer according to any one of claims 6 to 8, wherein:

10. A layer according to any one of claims 6 to 9, wherein the surface has an average grain size in the range of 0.2 μm to 25 μm.

11. 11. The layer according to claim 6, wherein the surface hardness of the layer is at least 0.5% higher than the cross-sectional hardness of the layer.

12. 12. The layer according to claim 6, wherein one surface of the layer has an average roughness Ra according to ISO 4287 in the nanoscale roughness range of 0.1 nm to 100 nm or in the microscale roughness range of 100 nm to 10 μm.

13. 13. The layer according to claim 6, wherein the layer has a thickness of 0.5 μm or more.

14. 14. A device for high temperature applications, comprising a layer according to any one of claims 6 to 13 on a surface of the device.

15. Use of a layer according to any one of claims 6 to 12 for supporting a semiconductor.

16. The device of claim 14, wherein the device is a wafer carrier.

17. The use of claim 15, wherein the layer is a free-standing layer and is used as a wafer for depositing a semiconductor.

Citation Information

Patent Citations

  • Production of rigid carbon film

    JP1988286576A

  • Manufacture of sic mask supporter for x-ray lithography mask

    JP1989112728A

  • Jig for semiconductor production and method for producing same

    US20120196038A1

  • Double isolation for electronic devices

    US3769562A

  • Jig for semiconductor production and method for producing same