Hot-rolled steel sheet for non-oriented electrical steel sheet and its manufacturing method
The hot-rolled steel sheet achieves both low iron loss and high magnetic flux density by controlling Ti precipitation through specific chemical composition and manufacturing processes, addressing the limitations of existing technologies in non-oriented electrical steel sheets.
Patent Information
- Application Number
- JP2023514245
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-04-14
- Publication Date
- 2024-12-04
- Estimated Expiration
- 2041-04-14
AI Technical Summary
Existing non-oriented electrical steel sheets face the challenge of achieving both low iron loss and high magnetic flux density, particularly in general-purpose grades with limited chemical components.
A hot-rolled steel sheet with controlled chemical composition and manufacturing processes, including specific temperature and rolling conditions, to precipitate Ti as Ti nitrides and Ti carbides, reducing solid solution Ti and stabilizing grain growth.
The solution enables both low iron loss and high magnetic flux density in non-oriented electrical steel sheets, even with limited chemical components, by stabilizing grain growth and controlling Ti precipitation.
Smart Images

Figure 0007594213000013 
Figure 0007594213000001 
Figure 0007594213000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a hot-rolled steel sheet for a non-oriented electrical steel sheet and a manufacturing method thereof. [Background technology]
[0002] In recent years, with the increasing demand for energy saving in electrical equipment worldwide, higher performance characteristics are being demanded for non-oriented electrical steel sheets used as iron core materials for rotating machines.
[0003] High-grade non-oriented electrical steel sheets are used for the highly efficient motors of electrical appliances. High-grade non-oriented electrical steel sheets generally have increased Si and Al contents to increase resistivity and have coarse grain sizes.
[0004] Meanwhile, general-purpose motors for electrical appliances use general-purpose grade non-oriented electrical steel sheets. In recent years, there has been a demand for improved performance for general-purpose motors, but because of strict cost constraints for general-purpose motors, it is difficult to switch to higher grade non-oriented electrical steel sheets, as is the case for high-efficiency motors.
[0005] General-purpose grade non-oriented electrical steel sheets generally have a chemical composition with a low Si content. In such general-purpose grade non-oriented electrical steel sheets, for example, the core loss characteristics can be improved by promoting grain growth during stress relief annealing performed after punching of motor cores.
[0006] As a method for improving grain growth during stress relief annealing, the following techniques have been proposed so far.
[0007] For example, Patent Document 1 discloses a method for producing an electric iron sheet having excellent magnetic properties, which comprises hot rolling a steel slab consisting of C; ≦0.065%, Si; ≦2.0%, Al; ≦0.10%, O; ≦0.020%, B / N; ≦0.50 to 2.50, the balance being Fe and unavoidable impurities, to obtain a hot-rolled sheet, which is then cold-rolled once or two or more times including intermediate annealing to obtain a final dimension, and then annealing the resulting sheet.
[0008] Patent Document 2 discloses a non-oriented electrical steel sheet containing 0.015% or less C, 0.1 to 1.0% Si, 0.001 to 0.005% sol. Al, 1.5% or less Mn, 0.008% or less S, 0.0050% or less N, and 0.02% or less TO, the non-oriented electrical steel sheet having low iron loss and capable of having an average crystal grain size of 50 μm or more after magnetic annealing, characterized in that the ratio of the weight of MnO to the total weight of three types of inclusions, SiO2, MnO, and Al2O3, in the steel is 15% or less.
[0009] In Patent Document 3, in a non-oriented electrical steel sheet containing, by weight, C: 0.01% or less, Si: 0.1% to 2.0%, Mn: 0.1% to 1.5%, and depending on the deoxidization method of the steel, Al: 0.1% or less or Zr: 0.05% or less, with the balance being iron and unavoidable impurity elements, the oxides in the steel having a diameter of 0.5 μm to 5 μm are found to be smaller than 1 cm 2 The number of particles per unit area is 1,000 to 50,000.
[0010] Patent Document 4 describes a steel containing, by mass%, C: 0.0050% or less, Si: 0.05 to 3.5%, Mn: 3.0% or less, Al: 3.0% or less, S: 0.008% or less, P: 0.15% or less, N: 0.0050% or less, and Cu: 0.2% or less, and satisfying (S which is Cu sulfide) / (S in steel)≦0.2 or (S which is Cu sulfide) / (S which is Mn sulfide)≦0.2, and further having a number density of Cu-containing sulfides having a diameter of 0.03 to 0.20 μm in the steel sheet of 0.5 pieces / μm. 3 The following non-oriented electrical steel sheet is disclosed.
[0011] In addition, Patent Document 5 describes a steel sheet containing, by mass%, Si: 1.5% or less, Mn: 0.4% or more and 1.5% or less, Sol.Al: 0.01% or more and 0.04% or less, Ti: 0.0015% or less, N: 0.0030% or less, S: 0.0010% or more and 0.0040% or less, B in terms of B / N of 0.5 or more and 1.5 or less, with the remainder being Fe and unavoidable impurities, and containing Mn, 10% or more of sulfides containing Mn are complex precipitates with B precipitates, and the total distribution density of MnS, CuS and their complex sulfides is 3.0×10 5 pieces / mm 2 The distribution density of Ti precipitates with a diameter of less than 0.1 μm is 1.0 × 10 3 pieces / mm 2 A non-oriented electrical steel sheet is disclosed, which is characterized in that: [Prior art documents] [Patent documents]
[0012] [Patent Document 1] Japanese Patent Publication No. 54-163720 [Patent Document 2] Japanese Patent Publication No. 63-195217 [Patent Document 3] Japanese Patent Publication No. 3-104844 [Patent Document 4] Japanese Patent Publication No. 2004-2954 [Patent Document 5] International Publication No. 2005 / 100627 Summary of the Invention [Problem to be solved by the invention]
[0013] The techniques of Patent Documents 1 to 5 promote the growth of crystal grains during stress relief annealing to reduce iron loss. However, these techniques have a new problem in that the magnetic flux density decreases as the iron loss is reduced. Thus, general-purpose grade non-oriented electrical steel sheets with limited chemical composition have a problem in that low iron loss and high magnetic flux density cannot be achieved at the same time at a high level.
[0014] The present invention has been made in view of the above problems, and aims to provide a hot-rolled steel sheet for non-oriented electrical steel sheet, which is capable of achieving both low core loss and high magnetic flux density even if the chemical composition is restricted, and a manufacturing method thereof. [Means for solving the problem]
[0015] The gist of the present invention is as follows.
[0016] (1) A hot-rolled steel sheet for non-oriented electrical steel sheet according to one aspect of the present invention is Chemical composition, by mass % C: 0.0010% or more and 0.0050% or less, Si: 0.1% or more and less than 0.5% Mn: 0.1% or more and 0.5% or less, Al: 0.1% or more and 0.5% or less, total-Ti: 0.0010% or more and 0.0030% or less, N: 0.0010% or more and 0.0030% or less, S: more than 0.0015% and less than 0.0040%, Nb: 0% or more and 0.0030% or less, V: 0% or more and 0.0030% or less, Zr: 0% or more and 0.0030% or less, Sn: 0% or more and 0.100% or less, with the remainder being Fe and impurities, The amount of solute Ti is 0.0005% or less, When observed on a surface parallel to the rolling direction and the sheet width direction, Ti carbides with a circle equivalent diameter of 10 nm to 50 nm are present within and at the grain boundaries of ferrite grains, 10% by number or more and 100% by number or less of the Ti carbides present in the grains are precipitated together with Mn sulfides, and The density of the Ti carbides present at the grain boundaries is 0.1 particles / μm or less. (2) The hot-rolled steel sheet for non-oriented electrical steel sheet described in (1) above is The chemical components are, in mass %, Sn: 0.010% or more and 0.100% or less may also contain (3) A method for producing a hot-rolled steel sheet for non-oriented electrical steel sheet according to one aspect of the present invention is a method for producing a hot-rolled steel sheet for non-oriented electrical steel sheet according to the above (1) or (2), Molten steel is cast and the chemical composition is calculated by mass %. C: 0.0010% or more and 0.0050% or less, Si: 0.1% or more and less than 0.5% Mn: 0.1% or more and 0.5% or less, Al: 0.1% or more and 0.5% or less, total-Ti: 0.0010% or more and 0.0030% or less, N: 0.0010% or more and 0.0030% or less, S: more than 0.0015% and less than 0.0040%, Nb: 0% or more and 0.0030% or less, V: 0% or more and 0.0030% or less, Zr: 0% or more and 0.0030% or less, Sn: 0% or more and 0.100% or less, a casting step for obtaining a slab containing the above-mentioned and the remainder being Fe and impurities; A hot rolling process of hot rolling the slab to obtain a hot rolled steel sheet, In the hot rolling process, Before hot rolling, the slab is heated and held at a temperature range of 1150°C to 1200°C for 10 minutes to 60 minutes; In the final pass of finishing hot rolling, a reduction of 20% to 30% is applied. After hot rolling, the steel sheet may be held within a temperature range of 800° C. or more and less than 900° C. for 15 minutes or more and 30 minutes or less. Effect of the Invention
[0017] According to the above-described aspects of the present invention, it is possible to provide a hot-rolled steel sheet for a non-oriented electrical steel sheet, which is capable of achieving both low core loss and high magnetic flux density even if the chemical components are restricted, and a manufacturing method thereof. [Brief description of the drawings]
[0018] [Figure 1] 1 is a graph showing the relationship between the amount of solute Ti in a hot-rolled steel sheet and the magnetic flux density B50 after stress relief annealing as a non-oriented electrical steel sheet. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] A preferred embodiment of the present invention will be described in detail below. However, the present invention is not limited to the configuration disclosed in this embodiment, and various modifications are possible without departing from the spirit of the present invention. In addition, the numerical ranges described below include lower and upper limits. Numerical values indicated as "more than" or "less than" are not included in the numerical range. In addition, unless otherwise specified, "%" regarding the content of each element means "mass %".
[0020] The present inventors have investigated the reason why the magnetic flux density after stress relief annealing is lower than that before stress relief annealing in Al-added steel containing about 0.002% Ti, focusing on the form of Ti.
[0021] In general, in Al-added steel, coarse AlN is likely to form during the steelmaking process or hot rolling process. The formed coarse AlN itself is not harmful to grain growth. However, when coarse AlN is formed, the N in the steel is reduced and the precipitation of TiN is suppressed. When the precipitation of TiN is suppressed in this way, the amount of solute Ti in the steel increases. The inventors have found that if the amount of solute Ti is high at the hot-rolled steel sheet stage, the magnetic flux density decreases when the steel is subjected to stress relief annealing as a non-oriented electrical steel sheet (see FIG. 1).
[0022] One method for reducing the amount of solute Ti in a hot-rolled steel sheet is to reduce the Ti content of the slab. If the Ti content of the slab is reduced, the amount of solute Ti in the hot-rolled steel sheet is also reduced, and as a result, the crystal grain growth during stress relief annealing of the non-oriented electrical steel sheet is stabilized, and the decrease in magnetic flux density after stress relief annealing is suppressed. However, Ti contained in the slab is an impurity element. Reducing the Ti content of the slab to an extent that the above-mentioned decrease in magnetic flux density can be avoided is not preferable because it increases the manufacturing cost of the non-oriented electrical steel sheet.
[0023] Therefore, the present inventors have intensively studied a method for obtaining good magnetic properties as a general-purpose grade non-oriented electrical steel sheet even if Ti is contained as an impurity in the slab. As a result, the present inventors have found that it is preferable to reduce the amount of Ti dissolved in the steel by precipitating Ti contained as an impurity as much as possible as Ti nitrides and Ti carbides at the stage of the hot-rolled steel sheet.
[0024] In addition, the inventors have found that while the Ti nitrides do not inhibit grain growth because the precipitate size is sufficiently large, it is not sufficient to simply precipitate the Ti carbides, and it is necessary to control the precipitation form. For example, the inventors have found that if Ti carbides are precipitated together with Mn sulfides at the stage of a hot-rolled steel sheet, and the number of Ti carbides precipitated alone at grain boundaries can be suppressed, the grains will grow stably when stress relief annealing is performed as a non-oriented electrical steel sheet. The idea behind this is shown below.
[0025] First, in order to reduce the amount of solute Ti in hot-rolled steel sheets, it is necessary to precipitate the Ti in the steel as Ti nitrides. As a result of the investigation, it was found that if the slab heating before hot rolling is properly controlled, TiN precipitates in preference to AlN, and the amount of solute Ti in the hot-rolled steel sheets can be reduced to a certain extent. In order to precipitate TiN in preference to AlN in this way, the slab should be heated to a temperature range of 1150°C to 1200°C before hot rolling and kept within this temperature range for 10 minutes to 60 minutes.
[0026] However, as described above, it is not enough to merely precipitate Ti in steel as Ti nitrides. In order to sufficiently reduce the amount of dissolved Ti in the hot-rolled steel sheet, it is necessary to further precipitate Ti in steel as Ti carbides. At this time, it is necessary to suppress the Ti carbides from precipitating alone at the ferrite grain boundaries by complexly precipitating them with Mn sulfides in the ferrite grains so as not to inhibit grain growth. As a result of the study, it was found that Ti carbides can be precipitated in a preferred form by controlling the reduction rate in the final pass of finish hot rolling and appropriately controlling the temperature of the steel sheet after hot rolling. In this way, in order to preferably precipitate Ti carbides, it is sufficient to apply a reduction rate of 20% to 30% in the final pass of finish hot rolling and hold the steel sheet after hot rolling in a temperature range of 800 ° C. to less than 900 ° C. for 15 minutes to 30 minutes.
[0027] As described above, the temperature control before hot rolling causes Ti in the steel to precipitate as TiN, and the rolling control in the final pass of finish hot rolling and the temperature control after hot rolling cause Ti in the steel to further precipitate as TiC. As a result, the amount of dissolved Ti in the hot-rolled steel sheet is reduced, and crystal grains grow stably when stress relief annealing is performed on the non-oriented electrical steel sheet, thereby realizing low iron loss and high magnetic flux density.
[0028] The TiN precipitated by temperature control before hot rolling has a sufficiently large precipitate size that it does not impede grain growth. On the other hand, TiC precipitated at grain boundaries significantly impairs grain growth, but TiC precipitated on Mn sulfides within grains does not impair grain growth. Therefore, it is necessary to suppress TiC from precipitating alone at ferrite grain boundaries by precipitating it together with sulfides within ferrite grains.
[0029] That is, in the hot-rolled steel sheet for grain-oriented electrical steel sheet according to the present embodiment, the amount of solute Ti is reduced by precipitating Ti in the steel as Ti nitrides and Ti carbides, and the precipitation form of Ti carbides is controlled so as not to inhibit grain growth. As a result, even if the chemical composition is limited as a general-purpose grade, low iron loss and high magnetic flux density can be achieved at a high level.
[0030] In addition, since the hot-rolled steel sheet for grain-oriented electrical steel sheet according to the present embodiment is premised on reducing the amount of solute Ti, it is preferable to reduce the contents of Nb, V, and Zr, which are nitride-forming elements other than Ti, so as not to unnecessarily consume N in the steel. For example, the contents of Nb, V, and Zr may each be 0.0030% or less.
[0031] <Chemical composition of hot-rolled steel sheet> First, with regard to the hot-rolled steel sheet for the non-oriented electrical steel sheet according to this embodiment, the reasons for limiting the chemical components of the steel will be described.
[0032] In this embodiment, the heat-rolled steel sheet contains, as its chemical components, basic elements, optional elements as necessary, and the balance being Fe and impurities.
[0033] C (carbon) is a basic element. If the C content is excessive, the core loss of the non-oriented electrical steel sheet is deteriorated by magnetic aging. Therefore, the C content is set to 0.0050% or less. On the other hand, from the viewpoint of avoiding the formation of solid solution B, the C content is set to 0.0010% or more. The C content may be set to 0.0045% or less, 0.0040% or less, or 0.0035% or less. The C content may also be set to 0.0015% or more, 0.0020% or more, or 0.0025% or more.
[0034] Si (silicon) is a basic element. Si is an effective element for increasing the electrical resistance of non-oriented electrical steel sheets. However, excessive Si content leads to an increase in hardness of the non-oriented electrical steel sheets, a decrease in magnetic flux density, and an increase in cost. As a chemical component of a general-purpose grade, the Si content is set to less than 0.5%. The Si content may be set to 0.4% or less. On the other hand, in order to obtain the above-mentioned effects, the Si content is set to 0.1% or more. The Si content may be set to 0.20% or more.
[0035] Mn (manganese) is a basic element. Mn is a sulfide-forming element, and it is preferable that an appropriate amount of Mn is included from the viewpoint of promoting grain growth. Therefore, the Mn content is set to 0.1% or more. The Mn content may be set to 0.20% or more. On the other hand, in consideration of the structure control of the hot-rolled sheet and the decrease in the saturation magnetic flux density of the non-oriented electrical steel sheet, the Mn content is set to 0.5% or less. The Mn content may be set to 0.4% or less.
[0036] Al (aluminum) is a basic element. Al is a deoxidizing element for steel. From the viewpoint of ensuring a stable deoxidizing effect and suppressing the generation of fine AlN, the Al content is set to 0.1% or more. On the other hand, if the Al content is excessive, AlN precipitates in preference to TiN, preventing the reduction of the amount of solid-solubilized Ti through TiN precipitation. Therefore, the Al content is set to 0.5% or less. More preferably, the Al content may be set to 0.3% or less, or 0.2% or less.
[0037] Ti (titanium) is an element mixed into slabs. Reducing the Ti content to zero leads to increased manufacturing costs. Therefore, as a chemical component of general-purpose grades, the total Ti content is set to 0.0010% or more. The total Ti content may be more than 0.0020%. On the other hand, if the total Ti content is excessive, it becomes difficult to reduce the amount of dissolved Ti. Therefore, the total Ti content is set to 0.0030% or less. Note that total Ti refers to the total Ti that is dissolved in steel and the Ti contained in precipitates such as TiN and TiC.
[0038] Nb (niobium) is an optional element. Nb generates nitrides and consumes N in steel, which may prevent the reduction of the amount of solid-solubilized Ti through the generation of TiN. However, Nb is an element that is mixed into slabs. Excessive reduction of the Nb content leads to an increase in manufacturing costs. Therefore, taking into consideration the generation of TiN and manufacturing costs, the Nb content is set to 0.0030% or less. More preferably, the Nb content may be set to 0.0025% or less, 0.0020% or less, or 0.0015% or less. The lower the Nb content, the more preferable it is, and the lower limit may be 0%. However, taking into consideration industrial productivity, the Nb content may be set to 0.0001% or more, 0.0005% or more, or 0.0010% or more.
[0039] V (vanadium) is an optional element. V generates nitrides and consumes N in the steel, which can prevent the reduction of the amount of dissolved Ti through the generation of TiN. However, V is an element that is mixed into the slab. Excessive reduction of the V content leads to an increase in manufacturing costs. Therefore, taking into consideration the generation of TiN and manufacturing costs, the V content is set to 0.0030% or less. More preferably, the V content may be set to 0.0025% or less, 0.0020% or less, or 0.0015% or less. The lower the V content, the more preferable it is, and the lower limit may be 0%. However, taking into consideration industrial productivity, the V content may be set to 0.0001% or more, 0.0005% or more, or 0.0010% or more.
[0040] Zr (zirconium) is an optional element. Zr generates nitrides and consumes N in steel, which can prevent the reduction of the amount of solid-solubilized Ti through the generation of TiN. However, Zr is an element that is mixed into slabs. Excessive reduction of the Zr content leads to an increase in manufacturing costs. Therefore, taking into consideration the generation of TiN and manufacturing costs, the Zr content is set to 0.0030% or less. More preferably, the Zr content may be set to 0.0025% or less, 0.0020% or less, or 0.0015% or less. The lower the Zr content, the more preferable it is, and the lower limit may be 0%. However, taking into consideration industrial productivity, the Zr content may be set to 0.0001% or more, 0.0005% or more, or 0.0010% or more.
[0041] N (nitrogen) is a basic element that forms nitrides. In general, in non-oriented electrical steel sheets, nitrides are considered to be harmful to grain growth. However, the present inventors have found that if N is used to fix Ti as Ti nitrides such as TiN and the amount of dissolved Ti in the hot-rolled steel sheet is reduced, the decrease in magnetic flux density after stress relief annealing can be suppressed. Therefore, the N content is set to 0.0010% or more. The N content may be set to 0.0012% or more, 0.0015% or more, or 0.0020% or more. On the other hand, excessive N is not preferable because it inhibits grain growth. Therefore, the N content is set to 0.0030% or less. The N content may be set to 0.0025% or less.
[0042] S (sulfur) is a basic element that forms Mn sulfides. In general, in non-oriented electrical steel sheets, it is believed that the S content should be reduced as much as possible because sulfides impair grain growth. However, the present inventor has found that an appropriate amount of sulfides functions as a precipitation nucleus for TiC and further renders TiC harmless. Ordinary TiC precipitates at the grain boundaries of ferrite grains before grain growth, significantly impairing grain growth. On the other hand, TiC precipitated on sulfides precipitates within the grains of ferrite grains, so does not impair grain growth. In order to precipitate TiC on sulfides, the S content is made to be more than 0.0015%. The S content may be 0.0020% or more, or may be more than 0.0020%. On the other hand, excessive S is undesirable because it inhibits grain growth. In particular, when the S content exceeds 0.0040%, the amount of sulfide precipitation increases, inhibiting grain growth. Therefore, the S content is set to 0.0040% or less. The S content may be set to 0.0035% or less, 0.0030% or less, or 0.0025% or less.
[0043] Sn (tin) is a selected element. The lower limit of the Sn content may be 0%. However, Sn has the effect of improving the magnetic flux density. In addition, Sn is also effective in suppressing nitridation and oxidation of the steel sheet surface during annealing. Therefore, Sn may be contained as necessary. For example, the Sn content may be 0.010% or more, 0.020% or more, or 0.050% or more. On the other hand, if the Sn content is too high, the effect will saturate, so the Sn content may be 0.100% or less, 0.090% or less, or 0.080% or less.
[0044] The balance of the chemical components consists of Fe and impurities. Note that the impurities mean elements that do not impair the effects of the present embodiment even if contained, and refer to elements mixed from ores or scraps as raw materials or from the manufacturing environment, etc. when industrially manufacturing the steel sheet. The upper limit of the total content of impurities may be, for example, 5%.
[0045] The above chemical components may be measured by a general analysis method for steel. For example, the chemical components may be measured using ICP-AES (Inductively Coupled Plasma-Atomic Emission Spectrometry). Specifically, a 35 mm square test piece collected from the steel sheet is measured under conditions based on a calibration curve created in advance by an ICPS-8100 or the like (measurement device) manufactured by Shimadzu Corporation, whereby the chemical components are specified. Note that C may be measured using the combustion-infrared absorption method, and N may be measured using the inert gas fusion-thermal conductivity method.
[0046] <Ti carbide> Next, regarding the hot-rolled steel sheet for non-oriented electrical steel sheets according to the present embodiment, the characteristics of Ti carbide (TiC) will be described.
[0047] As described above, in the present embodiment, the chemical components and the manufacturing conditions are controlled in a complex and inseparable manner to control the Ti precipitates contained in the hot-rolled steel sheet. In particular, in the present embodiment, the precipitation of Ti carbide alone at the grain boundaries of ferrite grains is suppressed.
[0048] In the hot-rolled steel sheet for non-oriented electrical steel sheet according to this embodiment, when observed on a surface parallel to the rolling direction and the sheet width direction, Ti carbides having a circle equivalent diameter of 10 nm or more and 50 nm or less are present within and on the grain boundaries of ferrite grains, 10% by number or more and 100% by number or less of the Ti carbides present in the grains are precipitated together with Mn sulfides, and The density of the Ti carbides present at the grain boundaries is 0.1 particles / μm or less.
[0049] In this embodiment, the size of Ti carbide that has the greatest effect on grain growth is controlled to be 10 nm or more and 50 nm or less in circle equivalent diameter. In the hot-rolled steel sheet for non-oriented electrical steel sheet according to this embodiment, Ti carbide of the above size is contained within and at the grain boundaries of ferrite grains.
[0050] If 10% by number or more and 100% by number or less of the Ti carbides present within the ferrite grains are precipitated in a composite manner with Mn sulfides, the number density of the Ti carbides present alone at the grain boundaries of the ferrite grains can be controlled to 0.1 / μm or less. It is preferable that 20% by number or more, 30% by number or more, 40% by number or more, or 50% by number or more of the Ti carbides present within the ferrite grains are precipitated in a composite manner with Mn sulfides.
[0051] If the number density of Ti carbides present at the grain boundaries of ferrite grains is 0.1 / μm or less, crystal grain growth is not hindered. The number density of Ti carbides present at the grain boundaries is preferably 0.05 / μm or less, 0.01 / μm or less, or 0.005 / μm or less. The smaller the number density of Ti carbides present at the grain boundaries, the more preferable it is, so the lower limit may be zero.
[0052] The method for analyzing Ti carbides present within and on the grain boundaries of ferrite grains is as follows. (1) A hot-rolled steel sheet is sheared in the rolling direction and width direction to obtain small pieces. The surface of the small pieces (the rolling surface parallel to the rolling direction and width direction) is polished to a desired depth, and the back surface of the small pieces (the opposite rolling surface) is also polished to make the small pieces into a thin film. (2) Observe the polished surface using a transmission electron microscope, and identify whether inclusions with an equivalent circle diameter of 10 nm or more and 50 nm or less are located within grains or at grain boundaries. (3) The composition of each inclusion is measured using an EDS (energy dispersive X-ray analyzer) attached to a transmission electron microscope. (4) Inclusions with an atomic ratio of Mn and S of approximately 1:1 are judged to be Mn sulfides, and inclusions with an atomic ratio of Ti and C of approximately 1:1 are judged to be Ti carbides, and the numbers of these are counted. In addition, the number of composite precipitates of the Mn sulfides and Ti carbides is counted. (5) Based on the above calculation results, the percentage of Ti carbides that are precipitated together with Mn sulfides within ferrite grains is calculated. (6) Similarly, the number density of Ti carbides that exist in contact with the grain boundaries of ferrite grains is calculated. This number density is the number of Ti carbides that exist in contact with the grain boundaries of ferrite grains divided by the total length of the grain boundaries. The area of the measurement region must be at least 100 μm 2 The total measurement area must be at least 100 μm 2 If this is the case, the number of measurement points and the size of the measurement field of view are not particularly limited.
[0053] <Solved Ti amount> Next, the amount of solute Ti in the hot-rolled steel sheet for the non-oriented electrical steel sheet according to this embodiment will be described.
[0054] In the hot-rolled steel sheet for non-oriented electrical steel sheet according to the present embodiment, the amount of solute Ti in the steel is reduced by precipitating Ti in the steel as Ti nitrides and Ti carbides. Specifically, in the hot-rolled steel sheet for non-oriented electrical steel sheet according to the present embodiment, the amount of solute Ti is 0.0005% or less by mass%. When the amount of solute Ti in the hot-rolled steel sheet is 0.0005% or less, even if the non-oriented electrical steel sheet is subjected to stress relief annealing, the decrease in magnetic flux density can be suppressed. That is, even if the chemical composition is limited as a general-purpose grade, low iron loss and high magnetic flux density can be simultaneously achieved at a high level. The amount of solute Ti is preferably 0.0003% or less, or 0.0001% or less. Since the smaller the value of the amount of solute Ti, the more preferable it is, the lower limit may be zero.
[0055] In order to reduce the amount of solute Ti, Ti in the steel is precipitated as Ti nitrides and Ti carbides, but the precipitate size of the Ti nitrides is large enough that they do not inhibit grain growth. Therefore, in the heat-rolled steel sheet for non-oriented electrical steel sheet according to this embodiment, the precipitation form of the Ti nitrides (e.g., grain size and number density) is not limited as long as the amount of solute Ti is 0.0005% or less. On the other hand, Ti carbides inhibit grain growth. Therefore, in the heat-rolled steel sheet for non-oriented electrical steel sheet according to this embodiment, in addition to the amount of solute Ti being 0.0005% or less, the precipitation form of the Ti carbides is controlled as described above.
[0056] The method for quantifying solute Ti is as follows. (1) The total Ti content (the total amount of Ti constituting Ti precipitates and dissolved Ti) of the hot-rolled steel sheet is determined by chemical analysis. (2) The hot-rolled steel sheet is dissolved by electrolysis and the residue is extracted. (3) The components of the residue are analyzed by ICP to determine the Ti content of the residue. (4) The value obtained by subtracting the Ti content of the Ti precipitates in the hot-rolled steel sheet from the total Ti content in the hot-rolled steel sheet is regarded as the amount of solute Ti in the hot-rolled steel sheet. In the electrolytic method, both Ti nitrides and Ti carbides can be extracted as residues, and therefore the difference between the Ti content of the residue obtained by the electrolytic method and the total Ti content of the hot-rolled steel sheet can be regarded as the amount of dissolved Ti in the hot-rolled steel sheet.
[0057] <Average grain size> In the hot-rolled steel sheet according to the present embodiment, the average grain size is not particularly specified. However, in the non-oriented electrical steel sheet subjected to punching, the smaller the average grain size, the less burrs are generated during punching and the better the workability. Therefore, in the non-oriented electrical steel sheet after the finish annealing and before the stress relief annealing, the average grain size may be 30 μm or less.
[0058] In order to make the average grain size of the non-oriented electrical steel sheet after finish annealing and before stress relief annealing 30 μm or less using the hot-rolled steel sheet according to this embodiment, a known technique can be appropriately used. The average grain size of the non-oriented electrical steel sheet after finish annealing and before stress relief annealing can be measured by observing the cross section of the steel sheet with an optical microscope and counting the grains passing through a straight line drawn in the sheet thickness direction (the so-called counting method specified in Annex B of JIS G 0551:2013).
[0059] <Method of manufacturing hot-rolled steel sheets> Next, a method for producing a hot-rolled steel sheet for a non-oriented electrical steel sheet according to this embodiment will be described.
[0060] The method for producing a hot-rolled steel sheet according to this embodiment is as follows: Molten steel is cast and the chemical composition is calculated by mass %. C: 0.0010% or more and 0.0050% or less, Si: 0.1% or more and less than 0.5% Mn: 0.1% or more and 0.5% or less, Al: 0.1% or more and 0.5% or less, total-Ti: 0.0010% or more and 0.0030% or less, N: 0.0010% or more and 0.0030% or less, S: more than 0.0015% and less than 0.0040%, Nb: 0% or more and 0.0030% or less, V: 0% or more and 0.0030% or less, Zr: 0% or more and 0.0030% or less, Sn: 0% or more and 0.100% or less, a casting step for obtaining a slab containing the above-mentioned and the remainder being Fe and impurities; A hot rolling process of hot rolling the slab to obtain a hot rolled steel sheet, In the above hot rolling process, Before hot rolling, the slab is heated and held at a temperature of 1150°C or more and 1200°C or less for 10 minutes or more and 60 minutes or less; In the final pass of finishing hot rolling, a reduction of 20% to 30% is applied. After hot rolling, the steel sheet is held within a temperature range of 800° C. or more and less than 900° C. for 15 minutes or more and 30 minutes or less.
[0061] In the casting process, a slab is obtained by casting molten steel that has been refined so that the chemical composition of the finally obtained hot-rolled steel sheet falls within the above-mentioned range. The chemical composition of the slab is the same as that of the above-mentioned hot-rolled steel sheet. In the hot-rolled steel sheet according to this embodiment, the amount of solute Ti is particularly important, but the amount of solute Ti is controlled in the subsequent hot rolling process or the like. Therefore, the manufacturing conditions in the steelmaking process are not particularly limited, and known conditions can be appropriately adopted.
[0062] In the hot rolling process, the slab after the casting process is hot rolled to obtain a hot rolled steel sheet. This hot rolling process is an important process for controlling precipitates in order to control the amount of solute Ti.
[0063] First, it is necessary to suppress the formation of AlN and promote the precipitation of TiN. For this purpose, the slab before hot rolling is heated to a temperature range of 1150°C to 1200°C and held at this temperature range for 10 minutes to 60 minutes, and then the slab is hot rolled.
[0064] Although this heating condition promotes the precipitation of TiN, some Ti remains in a solid solution state in the hot-rolled steel sheet (hot-rolled steel sheet) under this heating condition alone. Therefore, it is necessary to promote the precipitation of TiC. However, when precipitating TiC, it is necessary to control it so that TiC does not precipitate alone at the ferrite grain boundaries.
[0065] Therefore, the final pass of the finish hot rolling is subjected to a reduction of 20% to 30%, and the temperature is kept within a range of 800°C to 900°C after the hot rolling for 15 to 30 minutes. This allows TiC to precipitate as a composite with Mn sulfide precipitated during hot rolling. When the above conditions are satisfied, TiC can be suppressed from precipitating compositely with Mn sulfide in ferrite grains and TiC can be suppressed from precipitating alone at the ferrite grain boundaries. Specifically, the number ratio of TiC precipitated compositely with Mn sulfide in ferrite grains is 10% by number to 100% by number, and the number density of TiC precipitated alone at the ferrite grain boundaries is 0.1 pieces / μm or less. As a result of such precipitation control, the amount of solute Ti in the hot-rolled steel sheet can be reduced to 0.0005% or less. Therefore, the grain growth during stress relief annealing is stabilized, and low iron loss and high magnetic flux density can be achieved at a high level even if the chemical composition is limited as a general-purpose grade.
[0066] If the reduction rate of the final pass of the finish hot rolling is less than 20% or more than 30%, TiC precipitates finely alone, and the grain growth after stress relief annealing becomes unstable. If the temperature is held at 800°C or less after hot rolling, TiC precipitates finely alone, and the grain growth after stress relief annealing becomes unstable. On the other hand, if the temperature is held at more than 900°C, solute Ti cannot be precipitated. Even if the temperature is held at 800°C or more and 900°C or less, if the holding time is less than 15 minutes or more than 30 minutes, complex precipitation does not occur sufficiently, and the grain growth during stress relief annealing becomes unstable.
[0067] <Manufacturing method of non-oriented electrical steel sheet> Next, a method for manufacturing a non-oriented electrical steel sheet using a hot-rolled steel sheet for the non-oriented electrical steel sheet according to this embodiment will be described.
[0068] The manufacturing method of the non-oriented electrical steel sheet according to the present embodiment is a manufacturing method of the non-oriented electrical steel sheet using the above-mentioned hot-rolled steel sheet, The hot-rolled steel sheet manufactured under the above-mentioned manufacturing conditions is pickled and cold-rolled without hot-rolled sheet annealing, The cold-rolled material after the cold rolling may be heated at a heating rate of 20°C / sec or more and soaked at a temperature of 850°C or less.
[0069] As described above, the hot-rolled steel sheet produced through the casting process and the hot rolling process is subjected to the pickling process, the cold rolling (cold rolling) process, and the finish annealing process without being subjected to the hot-rolled sheet annealing. Among these processes, the conditions of the pickling process and the cold rolling process are not particularly limited, and known conditions can be appropriately used.
[0070] The finish annealing process is a process of heating, soaking, and cooling the cold-rolled steel sheet after the cold rolling process. The conditions in the finish annealing process are not particularly limited, and known conditions can be used as appropriate. However, by using the hot-rolled steel sheet for the non-oriented electrical steel sheet according to this embodiment and setting the heating rate of the steel sheet to 20° C. / sec or more in the heating process of the finish annealing process, the magnetic flux density of the non-oriented electrical steel sheet can be increased. Therefore, the heating rate in the heating process of the finish annealing process may be set to 20° C. / sec or more. Here, the heating rate is the difference between the heating start temperature and the soaking temperature of the hot-rolled steel sheet divided by the time from the heating start temperature to the soaking temperature, that is, the average heating rate from the heating start temperature to the soaking temperature.
[0071] Furthermore, it may be specified that the annealing temperature (soaking temperature) in the soaking process of the final annealing step does not exceed 850°C. If the annealing temperature exceeds 850°C, TiC in the composite precipitates of TiC and sulfides controlled in the hot rolling step will become solid solution Ti again, which may destabilize grain growth. Therefore, it is preferable that the heating rate in the heating process of the final annealing step is 20°C / sec or more, and the annealing temperature in the soaking process of the final annealing step is 850°C or less.
[0072] The non-oriented electrical steel sheet obtained through the above-mentioned process can be suitably used as a material for electric products such as motors. When manufacturing motor components, the non-oriented electrical steel sheet is subjected to mechanical processing such as punching and stress relief annealing. Standard stress relief annealing conditions are an annealing temperature of 750°C and a holding time of 2 hours. However, the annealing temperature and time may be appropriately changed in consideration of both equipment restrictions and the promotion of grain growth. EXAMPLES
[0073] The effects of one embodiment of the present invention will be described in more detail with reference to the following examples, but the conditions in the examples are merely examples of conditions adopted to confirm the feasibility and effects of the present invention, and the present invention is not limited to these examples. Various conditions may be adopted in the present invention as long as they do not deviate from the gist of the present invention and the object of the present invention is achieved.
[0074] The slab with the adjusted chemical composition was hot-rolled and coiled into a hot-rolled steel sheet with a thickness of 2.5 mm. Tables 1A and 1B show the chemical compositions of the hot-rolled steel sheet, and Tables 2A to 2E show the hot-rolling conditions. Except for the amount of dissolved Ti, the chemical compositions of the slab and the hot-rolled steel sheet were equivalent.
[0075] The produced hot-rolled steel sheets were analyzed for the amount of solute Ti and Ti carbides according to the above-mentioned methods, and the results are shown in Tables 3A to 3E.
[0076] In addition, the hot-rolled steel sheets were pickled and then cold-rolled to 0.5 mm to obtain cold-rolled steel sheets, which were then finish-annealed under the conditions shown in Tables 2A to 2E to obtain non-oriented electrical steel sheets.
[0077] In order to determine whether the various non-oriented electrical steel sheets obtained by the above-mentioned procedure are non-oriented electrical steel sheets having (A) low iron loss after stress relief annealing and (B) high magnetic flux density after stress relief annealing, characteristic evaluation was carried out according to the following procedure and pass / fail criteria.
[0078] (A) Iron loss after stress relief annealing The iron loss (W15 / 50, W15 / 60) of the steel sheets after stress relief annealing (annealing temperature 750℃ and holding time 2 hours) was measured in accordance with JIS C 2552:2014 "Non-oriented electrical steel strip." Then, iron loss separation was performed using the dual frequency method, and non-oriented electrical steel sheets with a W15 / 50 hysteresis loss of 2.6 W / kg or less after stress relief annealing were judged to have excellent iron loss characteristics after stress relief annealing. Dual Frequency Method Divide the iron loss value of W15 / 50 by frequency 50...α Divide the iron loss value of W15 / 60 by the frequency of 60... β Hysteresis loss of W15 / 50 = α x 50 - (β - α) x 250
[0079] (B) Magnetic flux density after stress relief annealing The magnetic flux density (B 50 ) was measured in accordance with JIS C 2552:2014 "Non-oriented electrical steel strip". And, the saturation magnetic flux density Bs of the steel sheet was measured. 50 B is the value obtained by dividing 50 A non-oriented electrical steel sheet having a / Bs of 0.820 or more was judged to have excellent magnetic flux density after stress relief annealing. The saturation magnetic flux density Bs of the steel sheet can be obtained by substituting the chemical components of the steel sheet into the following formula. Saturation magnetic flux density Bs = 2.1561-0.0413 x Si-0.0198 x Mn-0.0604 x Al
[0080] The above evaluation results are shown in Tables 3A to 3E. As shown in Tables 1A to 3E, the inventive examples satisfied the chemical composition, amount of dissolved Ti, and Ti carbide requirements, and therefore achieved both low iron loss and high magnetic flux density. In contrast, the comparative examples did not satisfy any of the chemical composition, amount of dissolved Ti, or Ti carbide requirements, and therefore did not achieve both low iron loss and high magnetic flux density.
[0081] [Table 1A]
[0082] [Table 1B]
[0083]
Table 2A
[0084]
Table 2B
[0085]
Table 2C
[0086]
Table 2D
[0087]
Table 2E
[0088]
Table 3A
[0089]
Table 3B
[0090]
Table 3C
[0091]
Table 3D
[0092]
Table 3E
[0093] According to the above-mentioned aspects of the present invention, it is possible to provide a hot-rolled steel sheet for a non-oriented electrical steel sheet, which can achieve both low core loss and high magnetic flux density even if the chemical composition is restricted, and a manufacturing method thereof, and therefore has high industrial applicability.
Claims
1. Chemical composition, by mass percent C: 0.0010% or more and 0.0050% or less, Si: 0.1% or more and less than 0.5% Mn: 0.1% or more and 0.5% or less, Al: 0.1% or more and 0.5% or less, total-Ti: 0.0010% or more and 0.0030% or less, N: 0.0010% or more and 0.0030% or less, S: more than 0.0015% and less than 0.0040%, Nb: 0% or more and 0.0030% or less, V: 0% or more and 0.0030% or less, Zr: 0% or more and 0.0030% or less, Sn: 0% or more and 0.100% or less, with the remainder being Fe and impurities; The amount of solute Ti is 0.0005% or less, When observed in a plane parallel to the rolling direction and the sheet width direction, Ti carbides having a circle equivalent diameter of 10 nm or more and 50 nm or less are present within and on the grain boundaries of ferrite grains, 10% by number or more and 100% by number or less of the Ti carbides present in the grains are precipitated together with Mn sulfides, and The number density of the Ti carbides present at the grain boundaries is 0.1 particles / μm or less. A hot-rolled steel sheet for non-oriented electrical steel sheet, characterized in that
2. The chemical components are, in mass %, Sn: 0.010% or more and 0.100% or less Contains The hot-rolled steel sheet for non-oriented electrical steel sheet according to claim 1 .
3. A method for producing a hot-rolled steel sheet for non-oriented electrical steel sheet according to claim 1 or 2, Molten steel is cast and the chemical composition is calculated by mass %. C: 0.0010% or more and 0.0050% or less, Si: 0.1% or more and less than 0.5% Mn: 0.1% or more and 0.5% or less, Al: 0.1% or more and 0.5% or less, total-Ti: 0.0010% or more and 0.0030% or less, N: 0.0010% or more and 0.0030% or less, S: more than 0.0015% and less than 0.0040%, Nb: 0% or more and 0.0030% or less, V: 0% or more and 0.0030% or less, Zr: 0% or more and 0.0030% or less, Sn: 0% or more and 0.100% or less, a casting step for obtaining a slab containing the above-mentioned and the remainder being Fe and impurities; A hot rolling process of hot rolling the slab to obtain a hot rolled steel sheet, In the hot rolling process, Before hot rolling, the slab is heated and held within a temperature range of 1150° C. to 1200° C. for 10 minutes to 60 minutes; In the final pass of finish hot rolling, a reduction of 20% to 30% is applied. After hot rolling, the steel sheet is held within a temperature range of 800° C. or more and less than 900° C. for 15 minutes or more and 30 minutes or less. The present invention relates to a method for producing a hot-rolled steel sheet for use as a non-oriented electrical steel sheet.
Citation Information
Patent Citations
Low-mark vanadium and titanium containing non-oriented electrical steel and manufacturing method thereof
CN101914732A
Hot-rolled plate normalizing process for improving electromagnetic performance of low-grade non-oriented electrical steel
CN105779731A
Production of electric iron plate with excellent magnetic property
JP1979163720A
Nonoriented electrical steel sheet having small iron loss after magnetic annealing
JP1988195217A
Nonoriented silicon steel sheet excellent in magnetic characteristics and its manufacture
JP1991104844A