Sacrificial anodes, cathodic protection methods, and concrete structures

The sacrificial anode's design with defined contact surface area and compressive strength ensures prolonged cathodic protection by stabilizing current supply, addressing macrocell corrosion in varying corrosive environments.

JP7594481B2Active Publication Date: 2024-12-04SUMITOMO OSAKA CEMENT CO LTD +2
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
JP2021055356
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-29
Publication Date
2024-12-04
Estimated Expiration
2041-03-29

AI Technical Summary

Technical Problem

Existing sacrificial anodes fail to maintain effective cathodic protection over a long period due to varying corrosive environments, leading to macrocell corrosion.

Method used

A sacrificial anode with a specific configuration, including an anode part made of a metal with higher ionization tendency, a backfill part with hydraulic material, and a connecting part, designed to maintain a contact surface area and compressive strength within certain ranges, ensuring stable current supply.

Benefits of technology

The anode configuration provides sustained cathodic protection by suppressing macrocell corrosion and maintaining effective current supply for an extended duration.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007594481000004
    Figure 0007594481000004
  • Figure 0007594481000005
    Figure 0007594481000005
  • Figure 0007594481000006
    Figure 0007594481000006
Patent Text Reader

Abstract

To provide a sacrificial anode capable of maintaining a good cathodic protection effect over a relatively long term.SOLUTION: A sacrificial anode installed in a concrete structure comprising a concrete portion formed using concrete and a metal material embedded in the concrete portion to supply an anti-corrosion current to the metal material, and includes an anode unit constituted by a metal having a higher ionization tendency than that of the metal material. and a backfill portion formed using a hydraulic material and containing the anode portion, in which the anode portion has a surface area of 7.5 cm2 or more and 15.0 cm2 or less per 1 cm3 and the compressive strength of the backfill portion is 3 N / mm2 or more and 10 N / mm2 or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a sacrificial anode used in an electrochemical protection method, a electrochemical protection method using the sacrificial anode, and a concrete structure in which the sacrificial anode is installed. [Background technology]

[0002] There is known a concrete structure having a concrete portion formed by using concrete and a metal material embedded in the concrete portion. For example, concrete structures include so-called reinforced concrete formed by embedding reinforcing bars as the metal material in the concrete portion, and shield tunnel segments having bolt boxes embedded in the ends as the metal material. In such concrete structures, the environment corroding the metal material may differ from part to part.

[0003] Taking reinforced concrete as an example, the deteriorated portion of the concrete is chipped off and the chipped portion is backfilled with a cross-section repair material (such as polymer cement mortar) that is highly resistant to deterioration (cross-section repair method). In this case, the corrosive environment (e.g., chloride ion amount, pH, etc.) of the metal material may be different between the portion backfilled with the cross-section repair material (hereinafter also referred to as the "cross-section repair portion") and the surrounding portion (hereinafter also referred to as the "concrete framework"). As a result, the metal material located on the cross-section repair portion side and the metal material located on the concrete framework side are exposed to different corrosive environments.

[0004] Taking the example of shield tunnel segments, the bolt box may be embedded with embedding material (e.g., cement mortar) after the segments are connected. In this case, the corrosive environment for metal materials (e.g., chloride ion amount, pH, etc.) may differ between the inside of the bolt box (embedding material) and the outside of the bolt box (concrete part). For this reason, the inside surface of the bolt box and the outside surface of the bolt box are exposed to different corrosive environments.

[0005] As described above, when the surface of a metal material is exposed to different corrosive environments in different parts, macrocell corrosion may occur on the surface of the metal material near the boundary between the corrosive environments. As a method for suppressing such macrocell corrosion, there is a method (electrochemical protection method) in which a sacrificial anode having a metal with a higher ionization tendency than the metal material as an anode part is installed in a concrete structure (see Patent Documents 1 to 8). In such an electrochemical protection method, a corrosion protection current is supplied from the sacrificial anode to the metal material, and the corrosion current generated in the metal material is suppressed, thereby suppressing the macrocell corrosion of the metal material.

[0006] Patent Documents 1, 2, 3, and 5 disclose cathodic protection methods in which the sacrificial anode itself has a special structure, and Patent Documents 4 and 8 disclose cathodic protection methods in which the installation position of the sacrificial anode is devised. Patent Document 6 discloses a cathodic protection method in which a paint made of finely powdered metal that will become the sacrificial anode is applied, and Patent Document 7 discloses a cathodic protection method in which the metal that will become the sacrificial anode is made into a blister shape. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Patent No. 3099830 [Patent Document 2] Patent No. 4574013 [Patent Document 3] Patent No. 4491139 [Patent Document 4] Patent No. 3556631 [Patent Document 5] Patent No. 4801051 [Patent Document 6] Patent No. 4648389 [Patent Document 7] Patent No. 5388435 [Patent Document 8] Patent No. 6325908 Summary of the Invention [Problem to be solved by the invention]

[0008] However, in recent years, in addition to the sacrificial anodes used in the above-mentioned conventional cathodic protection methods, there has been a demand for sacrificial anodes that can maintain a good cathodic protection effect for a relatively long period of time.

[0009] Therefore, an object of the present invention is to provide a sacrificial anode capable of maintaining a good cathodic protection effect for a relatively long period of time, and to provide a cathodic protection method using the sacrificial anode, and a concrete structure in which the sacrificial anode is installed. [Means for solving the problem]

[0010] The sacrificial anode according to the present invention is a sacrificial anode that is installed in a concrete structure having a concrete portion formed using concrete and a metal material embedded in the concrete portion to supply an anticorrosive current to the metal material, and is provided with an anode portion made of a metal having a higher ionization tendency than the metal material, and a backfill portion formed using a hydraulic material and containing the anode portion. 3 The surface area of ​​each piece is 7.5cm 2 More than 15.0cm 2 The compressive strength of the backfill is 3N / mm 2 More than 10N / mm 2 The following is the result.

[0011] With this configuration, the anode part is 1 cm 3 By setting the surface area per unit area and the compressive strength of the backfill portion within the above ranges, the cathodic protection effect can be maintained satisfactorily for a relatively long period of time.

[0012] The sacrificial anode according to the present invention has an anode part with a volume of 1 cm 3 More preferably, it is equal to or greater than this.

[0013] According to this configuration, since the volume of the anode portion is within the above range, the cathodic protection effect can be maintained satisfactorily for a longer period of time.

[0014] The cathodic protection method according to the present invention electrically connects the above-mentioned sacrificial anode to a metal material embedded in a concrete portion.

[0015] The concrete structure according to the present invention comprises a concrete portion formed using concrete, a metal material embedded in the concrete portion, and the above-mentioned sacrificial anode electrically connected to the metal material. Effect of the Invention

[0016] As described above, according to the present invention, the cathodic protection effect can be maintained satisfactorily for a relatively long period of time. [Brief description of the drawings]

[0017] [Figure 1] FIG. 2 is a perspective view showing the configuration of a sacrificial anode according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view showing the configuration of an electric protection method using a sacrificial anode according to the embodiment. [Diagram 3] FIG. 4 is a cross-sectional view showing the configuration of another electric protection method using a sacrificial anode according to the same embodiment. [Figure 4] FIG. 4 is a cross-sectional view showing the configuration of an electric corrosion protection method according to another embodiment. [Diagram 5] FIG. 11 is a cross-sectional view showing the configuration of an electric corrosion protection method according to yet another embodiment. [Figure 6] FIG. 2 is a cross-sectional view showing the configuration of a specimen for Test 1 of the embodiment. [Figure 7] FIG. 4 is a cross-sectional view showing the configuration of a specimen for Test 2 of the embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] Hereinafter, an embodiment of the present invention will be described with reference to FIGS. In the following drawings, the same or corresponding parts are given the same reference symbols and their descriptions will not be repeated.

[0019] The sacrificial anode 1 according to this embodiment shown in Fig. 1 is installed in a concrete structure including a concrete portion formed using concrete and a metal material embedded in the concrete portion, and supplies an anticorrosive current to the metal material to perform electrochemical protection of the metal material. The concrete portion is formed by kneading cement, coarse aggregate, fine aggregate, and water and allowing it to harden. The sacrificial anode 1 includes an anode part 2 made of a metal having a higher ionization tendency than the metal material, and a backfill part 3 containing the anode part 2. The sacrificial anode 1 further includes a connection part 4 that electrically connects the anode part 2 and the metal material.

[0020] The metal constituting the anode part 2 is not particularly limited, and examples thereof include zinc, zinc alloys, aluminum, aluminum alloys, indium, copper, and copper alloys. The zinc alloy contains Zn as the main component and at least one other metal such as Al, Cu, Mg, Fe, or In. The aluminum alloy contains Al as a main component and at least one other metal such as Zn, Mg, Cr, Si, or In. The copper alloy contains Cu as a main component and at least one other metal such as Ni, Zn, Sn, Al, or In. The metal constituting the anode part 2 can be appropriately selected depending on the metal constituting the metal material in the concrete structure. For example, when the metal material is a steel material (iron material), it is preferable to use zinc or a zinc alloy as the metal constituting the anode part 2, among metals composed of metals having a higher ionization tendency than the metal material, because they are easy to process and have a good balance between the supply amount and supply period of the anticorrosive current.

[0021] The shape of the anode part 2 is not particularly limited, and examples thereof include a mesh, plate, rod, and strip shape. The anode part 2 is 1 cm 3 The surface area of ​​each piece is 7.5cm 2 More than 15.0cm 2 Less than or equal to 10.0 cm, preferably 2 More than 12.5cm 2The surface area within the above range allows a stable supply of anticorrosive current from the anode part 2 to the metal material, and allows the supply to be continued for a relatively long period of time. The volume of the anode part 2 (the total volume of the anode part contained in the backfill part 3) is not particularly limited, and may be, for example, 1 cm 3 It is preferable that the length is at least 5 cm. 3 When the volume of the anode part 2 is in the above range, a corrosion protection current can be supplied to the metal material for a relatively long period of time.

[0022] The backfill portion 3 is formed using a hydraulic material. Specifically, the backfill portion 3 is formed by kneading the hydraulic material with water, forming a kneaded product, and then hardening the kneaded product to form a predetermined shape. The hydraulic material is not particularly limited, and examples thereof include at least one selected from the group consisting of cement, magnesium hydroxide, gypsum, dolomite, bentonite, and clay.

[0023] The compressive strength of the backfill portion 3 is 3N / mm 2 More than 10N / mm 2 The compressive strength of the backfill portion 3 can be measured by the method described in the following examples. 2 By satisfying the above, it is possible to suppress the occurrence of cracks in the backfill section 3. Specifically, when an anticorrosive current is supplied from the anode section 2 to the metal material, an oxide is generated, and when the molten oxide fills the voids in the backfill section 3, an expansion pressure is generated in the backfill section 3. However, when the compressive strength of the backfill section 3 is 3N / mm 2 By setting the compressive strength at or above 10 N / mm 2 , it is possible to suppress the occurrence of cracks in the backfill portion 3 due to the expansion pressure. 2 or less, there are a relatively large number of voids into which oxides generated when an anticorrosive current is supplied from the anode part 2 can dissolve. This makes it possible to prevent the surface of the anode part 2 from being covered with insoluble oxides early on, preventing the supply of an anticorrosive current.

[0024] The pH of the backfill part 3 is not particularly limited as long as it is within a range that can suppress passivation of the anode part 2. For example, when the anode part 2 is zinc or a zinc alloy, the pH of the backfill part 3 is preferably 13.3 or higher. When the pH of the backfill part 3 is within the above-mentioned numerical range, passivation of the anode part 2 can be suppressed.

[0025] The connection part 4 is formed using a material having electrical conductivity. Examples of materials constituting the connection part 4 include iron, stainless steel, and titanium. The shape of the connection part 4 is not particularly limited, and examples thereof include a line shape, a rod shape, and the like. In this embodiment, the connection part 4 is formed in a line shape. One end of the connection part 4 is connected to the anode part 2.

[0026] The method for producing the sacrificial anode 1 configured as above is not particularly limited, and for example, when cement is used as the hydraulic material forming the backfill portion 3, cement, fine aggregate, and water are mixed to form a mixture, and the anode portion 2 is embedded in the mixture so that the other end side of the connection portion 4 connected to the anode portion 2 is located outside the mixture. Then, the mixture is hardened to form the sacrificial anode 1 in which the anode portion 2 is embedded in the backfill portion 3 of a predetermined shape.

[0027] Next, a method for performing cathodic protection of a metal material embedded in a concrete structure (cathodic protection method) using the sacrificial anode 1 configured as above will be described. Specifically, as shown in Fig. 2, a method for performing cathodic protection of a concrete structure X (reinforced concrete) in which reinforcing bars are embedded as metal materials X1 in a concrete part X2 formed using concrete will be described. First, a part of the concrete part X2 in the concrete structure X is chipped away to form a recess X3, and a part of the metal material X1 is exposed inside the recess X3. Next, a sacrificial anode 1 is placed at the chipped portion, and the anode part 2 and the metal material X1 are electrically connected via a connection part 4. When connecting the anode part 2 and the metal material X1 via the connection part 4, a method of wrapping or welding the other end side of the connection part 4 around the metal material X1 can be adopted. Then, the recess X3 is backfilled with a cross-section repair material (mortar or the like) together with the sacrificial anode 1 to form a cross-section repair portion X4. In this way, a concrete structure X in which the sacrificial anode 1 is installed is formed. In the concrete structure X, a corrosion protection current is supplied to the metal material X1 with the metal material X1 serving as a cathode and the anode portion 2 of the sacrificial anode 1 serving as an anode, so that the metal material X1 can be electrically protected from corrosion.

[0028] Also, as shown in FIG. 3, a method of performing cathodic protection on a concrete structure X (such as a segment used in a shield tunnel) in which a metal bolt box X10 is embedded as a metal material X1 will be described. The bolt box X10 is embedded in a concrete part X2 at an end part of the concrete structure X. The bolt box X10 also includes box-shaped box bodies X10a and box connecting members X10b (specifically, bolts and nuts) that connect the box bodies X10a to each other. First, the sacrificial anode 1 is placed inside the box body X10a, and the box connecting member X10b (specifically, a bolt and a nut) and the anode part 2 are electrically connected via the connecting part 4. The box body X10a is then filled with a filling material (mortar or the like) to form the filling section X5. This forms a concrete structure X in which a sacrificial anode 1 is installed. In this concrete structure X, an anticorrosive current is supplied to the bolt box X10 with the bolt box X10 serving as a cathode and the anode section 2 of the sacrificial anode 1 serving as an anode. This allows cathodic protection of the bolt box X10.

[0029] As described above, the sacrificial anode, cathodic protection method, and concrete structure according to the present invention can maintain the cathodic protection effect well for a relatively long period of time.

[0030] That is, the sacrificial anode 1 according to this embodiment has a thickness of 1 cm 3 When the surface area per unit area and the compressive strength of the backfill portion 3 are within the above-mentioned ranges, the cathodic protection effect for the metal material X1 in the concrete structure X can be maintained satisfactorily for a relatively long period of time.

[0031] Furthermore, by having the volume of the anode portion 2 fall within the above range, the cathodic protection effect on the metal material X1 in the concrete structure X can be maintained satisfactorily for a longer period of time.

[0032] The sacrificial anode, cathodic protection method, and concrete structure according to the present invention are not limited to the above-mentioned embodiment, and various modifications are possible without departing from the gist of the present invention. Furthermore, it goes without saying that the configurations and methods of the above and following embodiments may be arbitrarily adopted and combined (the configurations and methods of one embodiment may be applied to the configurations and methods of other embodiments).

[0033] For example, in the above embodiment, the sacrificial anode 1 is configured to include a hardened backfill portion 3, but is not limited thereto, and for example, the backfill portion 3 may be in a freely deformable state (specifically, in a state before hardening). This allows the backfill portion 3 to be freely deformed, so that the backfill portion 3 can be formed into any shape and the sacrificial anode 1 can be installed in the concrete structure X.

[0034] In the above embodiment, the sacrificial anode 1 is formed with the anode portion 2 embedded in the backfill portion 3, and the sacrificial anode 1 is configured to be installed in the concrete structure X, but the present invention is not limited to this. For example, as shown in Fig. 4, the recess X3 may be backfilled with a backfilling material to the extent that the sacrificial anode 1 is not buried to form a cross-section repair portion X4, and the backfill portion 3 may be formed on the cross-section repair portion X4 to form the sacrificial anode 1. Alternatively, as shown in Fig. 5, the box body X10a may be embedded with an embedding material to the extent that the sacrificial anode 1 is not buried to form an embedding portion X5, and the backfill portion 3 may be formed on the embedding portion X5 to form the sacrificial anode 1.

[0035] In the above embodiment, the anode part 2 is electrically connected to the metal material X1 via the connection part 4, but this is not limited thereto. For example, the sacrificial anode 1 may be installed in the concrete structure X so that the anode part 2 is in direct contact with the metal material X1. In such a case, the sacrificial anode 1 may be configured not to include the connection part 4. EXAMPLES

[0036] The present invention will be described in more detail below using examples and comparative examples, but the present invention is not limited to the following examples.

[0037] <Backfill material (BF material)> Cement-based materials (manufactured by Sumitomo Osaka Cement Co., Ltd., product name: ordinary cement) Sodium hydroxide (first-class reagent) Lithium bromide (class 1 reagent)

[0038] <Anode material> Anode part A: A zinc alloy plate 3cm long, 3cm wide, and 0.54cm thick. Volume: 1cm 3 Surface area per 5.0cm 2 . Weight: 34.7g. Anode part B: A zinc alloy plate 4cm long, 4cm wide and 0.31cm thick. Volume: 1cm 3 Surface area per 7.5cm 2 . Weight: 35.4g. Anode part C: A zinc alloy plate 5cm long, 5cm wide and 0.20cm thick. Volume: 1cm 3 Surface area per 10.8cm 2 . Weight: 35.7g. Anode part D: Zinc alloy plate 6cm long, 6cm wide, 0.14cm thick. Volume: 1cm 3 Surface area per 15.0cm 2 . Mass: 36.0g. Anode part E: A zinc alloy plate measuring 7cm in length, 7cm in width and 0.10cm in thickness. Volume: 1cm 3 Surface area per 20.6cm 2 . Mass: 35.0g. Anode part F: An expanded metal net made from a zinc alloy plate measuring 3 cm in length, 5 cm in width and 0.32 cm in thickness. Volume: 1cm 3 Surface area per 12cm 2 . Weight: 34.3g. Anode part G: A zinc alloy plate measuring 2cm in length, 2cm in width and 0.20cm in thickness. Volume: 1cm 3 Surface area per 12.0cm 2 . Weight 5.7g. Anode part H: Zinc alloy plate 2cm long, 3cm wide and 0.20cm thick. Volume: 1cm 3 Surface area per 11.6cm 2 . Weight 8.6g. Anode part I: A zinc alloy plate 7cm long, 7cm wide, and 0.20cm thick. Volume: 1cm 3 Surface area per 10.6cm 2 . Mass: 70.0g.

[0039] 1. Test 1 <Preparation of sacrificial anode> A soft copper wire was connected to each anode part 2 as a connection part 4. The cement-based material was mixed with sodium hydroxide and lithium bromide and kneaded with water to prepare a BF material. The anode part 2 was then wrapped with the BF material to a thickness of 5 mm to form a backfill part 3, thereby preparing a sacrificial anode 1. The pH and compressive strength of the BF material (i.e., the backfill part 3) are shown in Table 1 below. The compressive strength was measured based on the "Method of compressive strength test for mortar or cement paste using cylindrical specimen (JSCE-G 505)".

[0040] <Preparation of specimen> As shown in Fig. 6, a concrete structure X (100 x 100 x 400 mm) was prepared as a test specimen, which included a plurality of metal materials X1 (four steel materials each having a diameter of 13 mm and a length of 80 mm), a concrete portion X2, a cross-section repair portion X4, and a sacrificial anode 1. The above test specimen was prepared in a thermostatic chamber at 20°C. Of the metal materials X1, the one located at the cross-section repair portion X4 was designated steel material No. 1, and the metal materials located away from steel material No. 1 were designated steel material No. 2, steel material No. 3, and steel material No. 4. Adjacent metal materials X1 were electrically insulated from each other by epoxy resin X6. In addition, adjacent metal materials X1 can be switched between an electrically connected state and an electrically disconnected state by switches S1 to S3. Moreover, the metal material X1 (steel material No. 1) located at the cross-section repair portion X4 and the sacrificial anode 1 are made switchable between an electrically connected state and an electrically disconnected state by the switch S4. The BF materials (A to E) and the anode parts 2 (A to I) used are shown in Table 2 below.

[0041] The concrete part X2 was prepared in the following manner. 3To obtain the above, sodium chloride (reagent) was added to ready-mixed concrete (manufactured by Sumitomo Osaka Cement Co., Ltd., called 21-18-20N) in a ratio of 60% water / cement to prepare a mixture. The mixture was then poured into a formwork in which metal material X1 (specifically, steel materials No. 2 to 4) was placed and allowed to harden. The mixture was then demolded 24 hours after pouring to obtain a concrete part X2.

[0042] The cross-sectional repair part X4 was prepared by the following method: Ordinary Portland cement (manufactured by Sumitomo Osaka Cement Co., Ltd.) was used as the cement, SBR latex (manufactured by Asahi Kasei Co., Ltd.) with a solid content of 45% was used as the polymer, and a mixed sand obtained by mixing equal amounts of silica sand No. 5 and silica sand No. 6 was used as the sand, with a polymer / cement ratio of 5%, a water / cement ratio of 45%, a sand / cement ratio of 2 / 1, and a chloride ion content of 0 kg / m 3 The mixture was prepared by the above method. A metal material X1 (specifically, steel material No. 1) was placed at a predetermined position of the concrete part X2 immediately after demolding, and the mixture was poured and hardened to form the cross-section repair part X4. When forming the cross-section repair part X4, the part of the concrete part X2 where the cross-section repair part X4 was to be formed (i.e., the surface in contact with the cross-section repair part X4) was roughened with sandpaper no. 60, and then the mixture for forming the cross-section repair part X4 was poured by only wetting with water without using a primer.

[0043] <Evaluation of corrosion level> The specimen (concrete structure X) prepared as described above was cured for 28 days after the casting of the cross-section repair section X4, by applying a wet cloth sufficiently saturated with water to the surface of the specimen, in a room at 20° C. During the curing period, the metal materials X1 were electrically connected to each other by the switches S1 to S3, and the sacrificial anode 1 and the steel material No. 1 were not electrically connected.

[0044] After the above curing was completed, the sacrificial anode 1 and the metal material X1 (steel material No. 1) were electrically connected by the switch S4, and the test specimen was then placed in a constant temperature and humidity chamber at 20° C. and 80% RH. Then, one month, one year, and two years after leaving the test specimen stationary, a zero-resistance ammeter was connected to switch S4 to measure the amount of protective current supplied from the sacrificial anode 1. The measurement results are shown in Table 2 below.

[0045] In addition, one month, one year, and two years after the specimens were left to stand, a non-resistance ammeter was connected to switches S1 to S3 to measure the natural potential of each metal material X1 (steel material No. 2 to No. 4). The natural potential was measured 24 hours after the electrical connection between the sacrificial anode 1 and steel material No. 1 was cut off by switch S4. The natural potential was measured in accordance with ASTM C876 using a saturated copper sulfate electrode as a reference electrode. By measuring such natural potential, the degree of corrosion of each metal material X1 can be grasped. Specifically, the more negative the natural potential is, the larger the potential difference occurring in the metal material X1 (i.e., the more corrosion current flows), and therefore the more advanced the corrosion of the metal material X1 is. Therefore, by measuring the above natural potential, the degree of corrosion of each metal material X1 (hereinafter, also referred to as "degree of corrosion") can be evaluated. The degree of corrosion was evaluated as follows: a natural potential of -350mV or less is x, a natural potential of more than -350mV and less than -200mV is △, and a natural potential of more than -200mV is ◯. The evaluation results are shown in Table 2 below.

[0046] 2. Test 2 <Preparation of specimen> As shown in Fig. 7, a bolt box X10 was used as the metal material X1. Two boxes, each 150 mm square and 100 mm deep, were made of a 3.2 mm thick black steel plate as the box body X10a. An M30 threaded steel bar and a hexagonal nut were used as the box connecting member X10b. The two box bodies X10a were integrated with the box connecting member X10b.

[0047] A sacrificial anode 1 having the anode portion 2 of C described above is placed inside the box body X10a, and a switch S5 makes it possible to switch between an electrically connected state and an electrically disconnected state between the sacrificial anode 1 and the bolt box X10 (box connecting member X10b). Thereafter, the above BF material was filled as an embedding material (mortar) in the box body X10a to form the embedding part X5, and the embedding part X5 was cured for 28 days to obtain the test specimen (concrete structure X). The embedding material (mortar) had a water / cement ratio of 50% and a sand / cement ratio of 3 / 1. The BF materials used are shown in Table 3 below.

[0048] <Corroded area rate> After the specimen was prepared, it was placed in a constant temperature room at 20°C and subjected to an accelerated corrosion test. The accelerated corrosion test consisted of spraying 1 liter of 2.5% sodium chloride solution on the specimen from the embedded part X5 side once a day and leaving it for 2 days, and this operation was repeated 5 times. One year after the start of the accelerated corrosion test, the specimen was destroyed to determine the corrosion area ratio inside the box body X10a. The corrosion area ratio is shown in Table 3 below. The corrosion area ratio is the ratio of the corroded area inside the box body X10a to the area of ​​the steel part inside the box body X10a.

[0049] [Table 1]

[0050] [Table 2]

[0051] [Table 3]

[0052] <Summary> As seen in Table 2, in each of the examples, the corrosion degree in the second year for Nos. 2 to 4 of the metal material X1 is "good", whereas in each of the comparative examples, the corrosion degree in the second year for any of Nos. 2 to 4 of the metal material X1 is "bad". 3 By setting the surface area per unit area and the compressive strength of the backfill portion 3 within the range of the present invention, even if there are portions within the concrete structure X that have different corrosive environments (specifically, the corrosive environment in the cross-section repair portion X4 and the corrosive environment in the concrete portion X2), corrosion of the metal material X1 can be suppressed for a relatively long period of time.

[0053] In addition, when Examples 7 to 10 in Table 2 are compared, it is found that in Example 7, the corrosion degree in the second year for Nos. 2 to 4 of the metal material X1 is "△", whereas in Examples 8 to 10, the corrosion degree in the second year for Nos. 2 to 4 of the metal material X1 is "◯". 3 By doing so, it is possible to suppress corrosion of the metal material X1 for a longer period of time.

[0054] Also, looking at Table 3, it is seen that the corrosion area ratio of each Example is smaller than that of each Comparative Example. 3 By setting the surface area per unit area and the compressive strength of the backfill portion 3 within the ranges of the present invention, a good cathodic protection effect can be obtained even in a concrete structure X other than so-called reinforced concrete. [Explanation of symbols]

[0055] 1...sacrificial anode, 2...anode part, 3...backfill part, 4...connection part, X...concrete structure, X1...metal material, X10...bolt box, X10a...box body, X10b...box connecting member, X2...concrete part, X3...recess, X4...cross-section repair part, X5...embedded part, X6...epoxy resin, S1 to S5...switch

Claims

1. A sacrificial anode that is installed in a concrete structure including a concrete portion formed using concrete and a metal material embedded in the concrete portion and supplies a corrosion protection current to the metal material, The anode portion is made of a metal having a higher ionization tendency than the metal material, and the backfill portion is made of a hydraulic material and contains the anode portion. The anode part is 1 cm 3 The surface area per unit is 7.5 cm 2 15.0cm or more 2 is as follows: The compressive strength of the backfill is 3N / mm 2 10N / mm or more 2 Is less than or equal to Sacrificial anode.

2. The volume of the anode is 1 cm 3 That's all. The sacrificial anode of claim 1.

3. The sacrificial anode according to claim 1 or 2 is electrically connected to a metal material embedded in a concrete portion. Electrical corrosion protection method.

4. A concrete portion formed by using concrete, a metal material embedded in the concrete portion, and the sacrificial anode according to claim 1 or 2 electrically connected to the metal material. Concrete structure.

Citation Information

Patent Citations

  • Generative method and device of heat for remoto heating by generating plant

    JP1978088435A

  • solenoid

    JP1988025908A

  • Anode assembly for cathode corrosion protection

    JP2008501859A

  • Concrete treatment methods

    JP2008533304A

  • Cross-sectional repair process for concrete structure

    JP2017014566A