Method for producing stainless steel strip
The method addresses the challenges of producing stainless steel strip by integrating hot and cold rolling with quenching and controlled descaling, achieving high-quality strips with fine surfaces and strength through a rolling mill line process.
Patent Information
- Application Number
- JP2021542109
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-01-28
- Filing Date
- 2020-01-24
- Publication Date
- 2024-12-04
- Estimated Expiration
- 2040-01-24
AI Technical Summary
Existing methods for producing stainless steel strip are costly and difficult to adapt to varying requirements for final product thickness, surface condition, and strength, particularly in integrated hot and cold rolling processes, with challenges in controlling oxide layers and mechanical stresses.
A method involving hot rolling followed by quenching to below 700°C, then cold rolling with initial cracks in the oxide layer to facilitate effective descaling and pickling, using a rolling mill line with specific annealing, descaling, and pickling steps to achieve high-quality stainless steel strip.
The method improves production efficiency, reduces oxide layer thickness, enhances surface quality, and increases the adaptability of rolling mill lines to produce stainless steel strips with fine surfaces and high strength, while minimizing mechanical stresses and production costs.
Smart Images

Figure 0007594532000002 
Figure 0007594532000003 
Figure 0007594532000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a stainless steel strip, which comprises rolling in the cold condition of a strip which has been produced in a preceding step through strip casting and / or hot rolling. The present invention also relates to a rolling mill line used during the implementation of the method. [Background technology]
[0002] Cold rolling of stainless steel strip is carried out for one or several purposes. The basic purpose is to reduce the thickness of the strip, usually as rolled in a previous hot rolling line, to a hot rolled strip thickness that is generally less than 1.5 mm, usually of the order of 2-6 mm, but may be up to 10 mm. Conventionally, an initial annealing, cooling, and pickling in one or more stages as well as descaling shot blasting precede the cold rolling, so as to obtain a starting material for cold rolling free of oxide and scale residues from the previous hot rolling. Alternatively, hot rolling may be completely or partially replaced by the production of the strip through casting, in which the strip may have a reduced thickness, not only to a thickness that is normal for hot rolled strip or several millimeters thicker, but in this case the initial annealing, cooling, descaling shot blasting, and pickling precede the cold rolling, to the extent that this technique has been performed in its entirety. Cold rolling, conventionally carried out in several uninterrupted cold rolling operations, possibly alternating with annealing, cooling, descaling and pickling operations, can reduce the thickness to gauges of 1 mm or even thinner. At the same time, these conventional cold rolling mills can produce strips with a very fine surface, the so-called 2B surface, if the rolling is completed by heat treatment, pickling and skin pass rolling, or even finer (BA surface), if bright annealing is employed. Cold rolling can also, as a main or additional objective, increase the strength of the strip material. For this purpose, as a complement to cold rolling, EP 0 738 781 also proposes cold drawing the strip, followed by annealing, so that the strip is plasticized and permanently elongated at the same time as its thickness is reduced. It is also known to carry out at least a first cold rolling operation on the cooled hot rolled strip or on the cooled cast strip, before heat treatment, pickling and possibly further cold rolling operations in order to bring the strip to the desired final gauge, as in US Patent No. 5,197,179 and EP Patent No. 0,837,147, although these are specific to the hitherto known methods and rolling mill lines which are expensive and / or difficult to meet the widely varying requirements as far as the thickness, surface condition and strength of the final product strip are concerned.This is especially true when hot rolling and subsequent cold rolling, as well as the operations associated with hot and cold rolling, are considered as an integrated production process. EP 1 637 243 discloses a method for producing stainless steel strip which involves hot rolling to a specified thickness followed by cold rolling to a thinner thickness, whereby this process involves two passes through a cold rolling line together with annealing and pickling. Summary of the Invention [Problem to be solved by the invention]
[0003] The object of the present invention is to address and resolve the above mentioned complexities. This can be achieved according to a first aspect of the invention in a manner consistent with the features according to claim 1.
[0004] As mentioned in the above description of the background of the invention, it is common to hot roll the strip to a final hot rolled strip gauge of 2-6 mm, and it is possible to hot roll down to 1.5 mm. The most complicated part of hot rolling is the final part, i.e. when hot rolling is performed on a rather thin strip. This stage is difficult to control and also results in a significant oxide on the strip, depending on the thickness of the strip. Also, the more the thickness of the strip is reduced, the less the yield in the production of the hot rolling mill is. In order to further improve the starting material used for the subsequent cold rolling, it is also advantageous to quench the strip from the final rolling temperature below 700 ° C, in order to avoid mechanical stresses and non-flatness of the hot strip during cooling, and in particular to increase the reproducibility during the process leading to the thinnest possible oxide layer on the one hand, and on the other hand to avoid the precipitation of grain boundary carbides in the surface layer. According to another aspect of the invention, the aim is to integrate the initial hot rolling and treatment of the strip, together with the hot rolling with subsequent cold rolling, so as to achieve a final product after cold rolling that is able to meet high requirements as far as excellent quality is concerned, with good production economy from an overall point of view, with increased capacity in the hot rolling mill, including less risk of failures in the hot rolling mill line. According to this aspect of the invention, the invention relates to a method for producing a stainless steel strip, comprising hot rolling in an initial step followed by cold rolling in a rolling mill line, characterized in that when the thickness of the strip has been reduced to a thickness of 2.0-6.5 mm, preferably 3-5 mm, the hot rolling is stopped and the strip thus hot rolled is cooled from the final hot / cold temperature through quenching to below 700°C and in the subsequent cold rolling is passed at least once through said cold rolling line comprising at least one cold rolling mill in the initial part of said line, and that after said initial cold rolling mill, at least one annealing zone and at least one pickling zone, when said strip passes for the first time through the at least one cold rolling mill in the initial part of said line, it is rolled with the dark oxide which it acquired in its hot condition during the initial step.
[0005] Initially, and optionally only in the cold rolling of stainless steel, if there is a dark oxide coating on both sides of the strip, this oxide coating, in combination with the initial process in the hot state of the steel, will form and cause some cracking of the oxide scale. This can be considered as an initial descaling action that can facilitate effective descaling that is carried out later, after annealing and before the strip is pickled. In order to allow the initial cracks to be effectively utilized to facilitate the later descaling and pickling, it is desirable to have the initial cracks eliminated as far as possible in combination with the annealing, i.e., the cracks or fissures in the oxide layer are not healed in the annealing. According to the invention, annealing is followed by a descaling step, followed by a scale breaker and shot blasting step. According to the invention, following the shot blasting step, the steel undergoes a pickling step using a combination of nitric acid, hydrofluoric acid, and optionally sulphuric acid. The elongation target of the scale breaker is set such that the flatness imperfections disappear after the cooling section (I) so that the strip is free of flatness imperfections before shot blasting, ensuring maximum shot blasting efficiency. The required stretch can be calculated as follows: Elongation (scale breaker) [%] = Elongation at yield point of material [%] + I / 10000 [%], where: (1) I = flatness defect defined in I-units; The I-unit is commonly used to define the height / wavelength relationship of flatness defects.
[0006] Further characteristics and aspects of the present invention will become apparent from the appended claims and from the following detailed description of the rolling mill line and how the invention can be reduced to practice in accordance with preferred embodiments. [Brief description of the drawings]
[0007] [Figure 1]FIG. 1 shows semi-schematically an embodiment of the invention and a rolling mill line. [Diagram 2] FIG. 2 shows very diagrammatically a preferred embodiment of the method for manufacturing the strip. [Diagram 3] FIG. 3 shows very diagrammatically a preferred embodiment of the method for manufacturing the strip. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] Figures 1 to 3 show diagrammatically several different methods for producing stainless steel strip. Austenitic or ferritic stainless steel strips preferably constitute the starting material for the process in the subsequent rolling mill line (Figures 2 and 3) used when carrying out the method according to the invention. Ferritic-austenitic steels are also conceivable. Three methods for producing the starting material are shown in Figure 1. According to method I, a slab 1 is hot rolled in a hot rolling mill line for the production of a hot rolled strip of a thickness that may be standard for hot rolled strips, i.e. a thickness of 1.5 to 6.5 mm. However, according to one aspect of the invention, the hot rolling is stopped before or at the latest when the thickness is reduced to 2.5 mm, so that the strip obtains a thickness within the standard dimensional range of 2 to 6.5 mm, preferably 3 to 5 mm. The hot rolled strip is quenched in a quenching section 3, preferably through an intense water spray, to a temperature below 700 ° C. The strip is then wound into a coil 4 and further cooled to below 100°C.
[0009] According to method II, the stainless steel strip is cast in strip form according to any technique that may be known per se and that, as far as its specific operating mode is concerned, does not form part of the present invention and will therefore not be described in more detail. However, by way of example, the so-called stainless steel strip casting by twin rolls, a technique known to those skilled in the art, can be used. The cast stainless steel strip is hot rolled in a hot rolling mill line 2' to a thickness that is conventional for stainless hot rolled strip or a slightly thicker thickness of 2 to 6 mm (see above), at which point the strip is immediately quenched in a cooling section 3 and wound to form a coil 4.
[0010] According to method III, the stainless steel strip is cast in the form of a strip having a thickness that is standard for stainless steel strip or possibly a slightly greater thickness, i.e., about 1.5 to 6.5 mm, at which point the strip is quenched in a cooling section 3' to a temperature below 700°C. The strip thus produced is wound into a coil 4'.
[0011] The starting material for the subsequent operations in the rolling mill line (Figures 2 and 3) consists of the thus cast and / or hot rolled stainless steel strip 4, 4'. Such a coil 4, 4' of stainless steel strip is shown in the figures as it unwinds from a decoiler 6. The auxiliary decoiler is indicated as 6A. A welder for joining the strip, a first strip looper and a first multi-roll S-mill are indicated as 7, 8 and 9, respectively. Then follows the initial cold rolling section 10, consisting of three cold rolling mills 11, 12, 13, which are of the so-called Z-high or 6-high type, meaning that each of them has a pair of a work roll and two support rolls, respectively above and below the work roll.
[0012] The initial cold rolling section 10 is followed by a degreasing machine 14, a second multi-roll S-mill 15, and a second band looper 16.
[0013] The strip unwound from the coil 6 is designated 5. After passing through the initial cold rolling section 10, the strip is designated 5'. From the strip looper 16, the strip 5' is fed into the annealing furnace 7 and into a cooling section consisting of two cooling chambers 18 and 19. It is then followed by a third multi-roll S-mill 20, a descaler 21 and a shot blasting stage 23. On either side of the descaler 21 there is a fourth multi-mill 20 and a fifth multi-mill 22, respectively. According to the invention, the descaler before the shot blasting device has the function of increasing the flatness of the metal strip, introducing primary cracks and increasing the effectiveness of the shot blasting stage.
[0014] The descaler 21 consists of a cold stretching mill, the design of which is shown in detail in FIG. 3 in the above-mentioned EP 0 738 781, which is incorporated herein by reference. This type of cold stretching mill comprises a series of rolls which alternately bend the strip in different directions as it is permanently lengthened through cold stretching. It has been found that it is possible to achieve effective descaling with this type of cold stretching mill without damaging the surface of the strip beneath the oxide layer.
[0015] The shot blast unit is followed by a pickling section which may consist, for example, of an initial neolyte or other electrolytic pickling section 26 and a mixed acid pickling section 27. The acid mixture consists of nitric acid HNO3, and hydrofluoric acid HF, and optionally sulfuric acid H2SO4. The pickled strip, designated 5'' may then be placed in a third strip looper 28.
[0016] A further terminal cold rolling mill is indicated as 32. This mill, according to this embodiment, consists of a four-high mill, i.e. a rolling mill with pairs of work rolls and support rolls above and below the work rolls respectively, allowing rolling with a reduction of up to 15-20%, depending on the type of stainless steel (austenitic or ferritic, ferritic steels can usually be rolled with a higher percentage reduction than austenitic steels). Alternatively, the finishing cold rolling mill can consist of a two-high mill intended only for skin-pass rolling. Following the rolling mill 32, a sixth multi-roll straightening mill 34 is provided before the strip 5''' is wound to form a coil 40 on a coiler 38. The auxiliary coiler is indicated as 38A.
[0017] According to various aspects of the invention, the stainless steel strip passes through the rolling mill line of Figure 2 at least once. According to a preferred embodiment, the strip passes through the rolling mill line twice. This will now be disclosed in more detail in connection with Figure 3, in which only the most basic equipment is shown, other components such as welding machines, S-mills, deflection and guide rollers, loopers, etc. have been omitted so that the principles of the invention become more clear. The reference numbers in parentheses indicate the strip material that is processed as it passes through the rolling mill line B for the second time.
[0018] Rolling in the rolling mill line starts by unwinding the hot-rolled or cast strip 5 of stainless steel from the coil 4, 4' of strip material. The strip still has its dark oxide coating that it acquired in the previous step in part A. This strip is cold rolled with a total thickness reduction of at least 10% and at most 75%, preferably 20-50% area reduction, in one, two or all three of the rolling mills 11, 12, 13 in the initial cold rolling section 10. The relatively thin dark oxide layer on the strip surface, obtained in the quench after hot rolling or casting, is so ductile that it does not break apart through the cold rolling action in the initial cold rolling section 10 to such an extent that the oxide layer loosens from the substrate, i.e. from the metal surface. However, fissures form in the oxide layer, i.e. the scale on the steel strip cracks. This is of essential importance for the subsequent pickling, where its effectiveness is promoted, which in turn is important for the realization of a fine surface in the final product.
[0019] In the annealing furnace 17, the strip 5' thus cold rolled is annealed by heating to a temperature within the range 780-1200°C depending on the steel grade for a time long enough for the strip to be fully heated and recrystallized, and a grain size model is applied to control the strip at that temperature.
[0020] In the cooling chamber 19, the strip 5' is cooled to below 100°C before being stretched in a descaler 21 between multiple rolls under repeated bending, thereby destroying the oxide scale and achieving good flatness. The strip is then shot blasted in the shot blasting section 23, which is a second treatment for the removal of oxides and scale from the strip surface. Descaling and subsequent shot blasting are preparatory steps for pickling in pickling units 26 and 27 in which the oxide scale is completely removed. The surface of the strip after the drawing mill 21 is shot blasted in a shot blasting unit 23 with steel shots before being pickled, first through section 26 and then electrolytic pickling in a mixed acid, which is a mixture of nitric acid (HNO3), hydrofluoric acid (HF) and optionally sulphuric acid (H2SO4).
[0021] The strip 5'' thus pickled is then cold rolled in an additional cold rolling mill 32 at the end where the strip 5'' is shaped to dimensions such that it can be further reduced in thickness by up to 20%. It is preferred that the strip gauge reduction in the finishing cold rolling mill 32 is at least 3%, and typically less than 15%. The strip 5''' is then wound to form a strip coil 40.
[0022] Descaling in the cold stretching mill 21 may be omitted entirely or cold stretching is performed to only a small extent, about 0.4-2%, although more extensive cold rolling, preferably less than 3%, is also conceivable according to certain embodiments of the invention. The strip is then pickled in pickling sections 26, 27 and finally wound into a coil.
[0023] According to one aspect of the invention, the ribbon is passed once more through the rolling mill line in the same direction as in the first pass. According to another aspect of the invention, the product from the first pass is the final product.
[0024] According to one embodiment of the invention, the strip coil 40, after a certain period of time, in particular a period determined by the logistics of production at the facility, is conveyed to the decoiler 6 or 6A at the beginning of the rolling mill line, where the strip (5''') is uncoiled again in a second pass of the strip through the rolling mill line. Whereas in the first pass the strip was possibly only rolled in one or two of the rolling mills 11-13 in the initial cold rolling section 10, this time it is rolled in two or three of the mills 11-13 so as to essentially achieve the desired final gauge of the strip. The total thickness reduction in the rolling mill section 10 in the second pass of the strip through this section can amount to 60% in total and at least 20%, preferably at least 30%. After the second pass through the cold rolling section 10, the strip (5''') is now uncoiled again. V ) is finished. The final treatment consists of passing the strip again through the annealing furnace 18, the cooling chambers 18 and 19 and the pickling sections 26 and 27. However, this time the strip is not treated at all in the descaler 21 or in the shot blasting unit 23, since neither descaling in the cold drawing mill 21 nor blasting in the blasting mill 23 is necessary, since the oxidation of the strip surface in this case is not significant. The annealed strip can then be pickled in the pickling units 26 and 27 immediately after cooling. This treatment is finished by skin pass rolling in the cold rolling mill 32 to a reduction of 0.2 to 1.5%, preferably about 0.5%, or by hard rolling to a reduction of 2 to 20%, preferably 10 to 15%, and / or by stretching through a stretching in the straightening mill 34 before the final coiling.
[0025] Obi (5 V ) may not be skin pass rolled if the objective is to produce a strip with very high yield strength, but may instead be rolled with the same large thickness reduction as when the strip was first rolled in the terminal cold rolling mill 32.
[0026] The above detailed description depicts preferred embodiments of the various aspects of the method of using the rolling mill line (FIGS. 2 and 3). It is a particular advantage of the design of the rolling mill line, or parts thereof, that in the production, the rolling mill line can be used in processes aiming not only at strips with a very fine bright surface, but also at strips with features that are more important than a very bright surface, such as strips with high strength, or strips with less improvement but with cost advantages, in some applications. For the latter purpose, the treatment may be stopped, for example, already after the strip 5'' has passed through the pickling zones 26, 27, after the first pass of the initial cold rolling zone 10, the annealing and cooling zones and the pickling zone. If it is desired to increase the strength, a 2-20% cold rolling may be performed in the final cold rolling mill 32, which in this case is performed on a non-lubricated surface, as the strip passes through the final cold rolling mill for the first time and then the process is finished by coiling the strip.
[0027] These examples and alternative methods exemplify the versatility and adaptability of rolling mill lines to different needs as far as the end product is concerned. EXAMPLES
[0028] A slab of stainless steel of grade ASTM 304 is hot rolled in a tandem mill to obtain a strip of width 1530 mm and thickness 6.5 mm. Once rolled, the strip is quenched from the final rolling temperature of about 900° C. to above 650° C. for about 10 seconds with water spray, after which the strip is coiled. This concept works well with normal hot zone cooling since grain boundary carbides can be controlled by annealing under conditions described in the examples above and pickling at standard scale levels.
[0029] The strip coil is then transported to the rolling mill line of the invention, unwound and cold rolled first in two of the rolling mills 11-13 in the initial cold rolling section 10 to a thickness of 3.0 mm with its dark oxide layer, which cracks but does not loosen. After this, the strip is annealed in the previously mentioned annealing furnace at a temperature of 1120° C. for a fairly long time in order to fully recrystallize it, after which the strip is cooled to below 100° C. in the cooling chambers 18 and 19. The strip then undergoes descaling in the drawing mill 21, after which the surface of the strip is shot blasted with steel shot in the shot blasting unit 23, before pickling the strip through electrolytic pickling in a mixed acid (a mixture of nitric acid HNO3, hydrofluoric acid HF and sulfuric acid H2SO4) first in section 26 and then in the pickling section 27. In the finishing cold rolling mill 32, the pickled strip is then cold rolled with a 10.0% thickness reduction to a gauge of 2.7 mm, after which the strip is coiled.
[0030] The strip is then returned to the starting position. Due to the intense cold rolling that the strip has undergone in the terminal cold rolling action in the rolling mill 32, the strip is deformation hardened to a considerable extent, so that it is not easily damaged and can therefore be transported and handled without the risk of damaging the strip surface. The strip is thus unwound again and this time rolled in all three rolling mills 11-13 of the initial cold rolling mill 10 with a total thickness reduction of 37% to the standard dimension of 1.7 mm. According to this example, the strip is annealed, cooled and then pickled as in the first pass through the rolling mill line, but without shot blasting or cold drawing before pickling. Finally, the strip is skin pass rolled in the terminal cold rolling mill 32 with a further thickness reduction of about 0.5%, so that the strip achieves a surface fineness of Ra 0.2 μm, i.e. a surface fineness that corresponds quite well to a 2B-surface.
[0031] As can be seen from the above, the cold rolling mill of the present invention is extremely versatile as far as its use is concerned for the production of stainless steel strip having a fine surface and / or for strip having other desirable qualities or characteristics. Table 1 below lists some of these alternative methods of producing strip in relation to the use of various thickness reduction units contained in a rolling mill line, i.e., an initial cold rolling mill, a descaler / cold drawing mill that may also be used to reduce the thickness of the strip, and a cold rolling mill, or in some cases multiple cold rolling mills terminating the line. [Table 1]
Claims
1. A method for producing a stainless steel strip, comprising hot rolling in an initial step (A) followed by cold rolling in a cold rolling line (B), wherein when the thickness of the strip is reduced to a thickness of 1.5 to 6.5 mm, the hot rolling is stopped and the strip is passed through the cold rolling line at least once in the subsequent cold rolling, the subsequent cold rolling being carried out in at least one cold rolling mill (11-13) in the initial part of the line and at least one annealing zone (14) after the at least one cold rolling mill(s) in the initial part of the line. a scale breaking stage (21), a shot blasting stage (23) and at least one pickling section (26, 27) using a mixture of acids in that order, the strip being rolled with dark residual oxides obtained in the hot condition of the strip during said initial steps when the strip passes for the first time through said at least one cold rolling mill of said initial part of the line, the method further comprising the steps of: cooling the hot rolled strip from the final hot rolling temperature through quenching to below 700° C.; and pickling with nitric acid (HNO 3 ) or nitric acid (HNO 4 ) or nitric acid (HNO 5 ) or nitric acid (HNO 6 ) or nitric acid (HNO 4 ) or nitric acid (HNO 5 ). 3 , hydrofluoric acid HF, and sulfuric acid H 2 SO 4 The method of claim 1, further comprising:
2. 2. The method of claim 1, characterized in that the thickness of the stainless steel strip is reduced by 10-60% when the stainless steel strip passes through the at least one cold rolling mill (11-13) for the first time and by up to 15% when the stainless steel strip passes through a terminal cold rolling mill (32) for the first time.
3. 3. The method of claim 2, wherein the strip is cold rolled and the thickness of the strip is reduced by at least 3% and at most 12% when the strip passes through the terminal cold rolling mill (32) for the first time.
4. 4. The method of claim 3, wherein the thickness of the band is reduced by at least 8%.
5. 5. The method according to any one of claims 1 to 4, characterized in that the thickness of the strip is reduced by 20 to 60% when the strip passes through the at least one cold rolling mill (11-13) for the second time.
6. A method according to any one of claims 2 to 5, characterised in that the strip is skin pass rolled by 0.5% during the second pass of the strip through the terminal cold rolling mill (32).
7. A method according to any one of the preceding claims, characterised in that the strip is cold rolled by 2-15% during the second pass of the strip through the terminal cold rolling mill (32).
8. A method according to any one of the preceding claims, characterised in that the strip is cold rolled by 8-12% during the second pass of the strip through the terminal cold rolling mill (32).
Citation Information
Patent Citations
Method for continuously manufacturing cold-rolled steel
EP2067541A1
Production of steel sheet for heat treatment excellent in peeling resistance of scale
JP1997256067A
Production of austenitic stainless steel sheet for roll forming
JP1998130734A
Strip manufacturing method and rolling mill line
JP2002532254A
Method for manufacturing stainless steel strips and integrated rolling mill line
JP2002532633A