Electrically heated carrier and exhaust gas purification device
By integrating an oxidation-preventing layer to shield the joint between the base layer and metal electrode, the EHCs overcome oxidation issues, ensuring durability and performance in high-temperature exhaust gas environments.
Patent Information
- Application Number
- JP2021561152
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-11-28
- Filing Date
- 2020-07-06
- Publication Date
- 2024-12-04
- Estimated Expiration
- 2040-07-06
AI Technical Summary
Existing electrically heated catalysts (EHCs) face issues with oxidation resistance at the bonding sites due to exposure to high temperatures in exhaust gas environments, leading to decreased strength and potential damage.
Incorporation of an oxidation-preventing layer to protect the joint between the base layer and metal electrode, using materials like ceramics or glass-based composites to seal and shield the bonding area from exhaust gases.
Effectively suppresses oxidation at the bonding site, maintaining structural integrity and preventing cracks, thereby enhancing the durability and performance of the EHCs.
Smart Images

Figure 0007594544000002 
Figure 0007594544000003 
Figure 0007594544000004
Abstract
Description
[Technical Field]
[0001] The present invention relates to an electrically heated carrier and an exhaust gas purification device. [Background technology]
[0002] In recent years, electrically heated catalysts (EHCs) have been proposed to alleviate the decline in exhaust gas purification performance immediately after engine start. EHCs are constructed by connecting metal electrodes to a columnar honeycomb structure made of conductive ceramics, and by passing electricity through the honeycomb structure itself, the honeycomb structure can generate heat and reach the catalyst's activation temperature before the engine starts. To fully utilize the catalytic effect of EHCs, it is desirable to minimize temperature variations within the honeycomb structure and achieve a uniform temperature distribution.
[0003] To pass current through an EHC, metal electrodes connected to external wiring must be bonded to the EHC by methods such as thermal spraying, laser welding, or brazing.
[0004] Patent Document 1 also discloses a technique for applying heat energy from the metal terminal (metal electrode) side to join a metal electrode onto an electrode layer of a honeycomb structure by welding. It also states that this configuration can provide a conductive honeycomb structure with improved joining reliability with the metal electrode. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 2018-172258 Summary of the Invention [Problem to be solved by the invention]
[0006] In Patent Document 1, a stress relief layer (base layer) is provided on the electrode layer to reduce breakage during welding and repeated fatigue of the ceramic honeycomb structure due to thermal cycles. However, EHCs are typically used at high temperatures (800 to 1000°C) in an exhaust gas atmosphere from automobiles, etc., and the physical properties of joints such as welded parts are changed by the energy generated during joining. Therefore, when these joints are exposed to exhaust gas from automobiles, etc., their oxidation resistance is likely to decrease. As a result, although stress relief is possible with the base layer, the material strength decreases due to oxidation, which can lead to problems such as breakage of the joints.
[0007] The present invention was created in consideration of the above circumstances, and aims to provide an electrically heated carrier and an exhaust gas purification device that can effectively suppress oxidation of the joint portion connecting the base layer and the metal electrode. Another aim of the present invention is to provide an electrically heated carrier and an exhaust gas purification device that can effectively suppress oxidation of the fixing layer that fixes the metal electrode to the electrode layer. [Means for solving the problem]
[0008] As a result of extensive research, the present inventors have found that the above-mentioned problems can be solved by providing an anti-oxidation layer to protect the joint between the base layer and the metal electrode from exhaust gas. That is, the present invention is specified as follows. (1) A ceramic pillar-shaped honeycomb structure having an outer peripheral wall and partition walls disposed inside the outer peripheral wall and defining a plurality of cells that form flow paths penetrating from one end face to the other end face; an electrode layer disposed on the surface of the outer wall of the pillar-shaped honeycomb structure; a conductive base layer provided on the electrode layer; a metal electrode connected to the underlayer by a bonding site; an anti-oxidation layer for protecting the bonding portion from exhaust gas; Electrically heated carrier with (2) A ceramic pillar-shaped honeycomb structure having an outer peripheral wall and partition walls disposed inside the outer peripheral wall and defining a plurality of cells that form flow paths penetrating from one end face to the other end face; an electrode layer disposed on the surface of the outer wall of the pillar-shaped honeycomb structure; a metal electrode provided on the electrode layer; a fixing layer provided to cover the metal electrode and fixing the metal electrode to the electrode layer; an antioxidant layer provided to cover the fixing layer; Electrically heated carrier with (3) An electrically heated carrier according to (1) or (2), a metallic cylindrical member for holding the electrically heated carrier; An exhaust gas purification device having the above structure. [Effects of the Invention]
[0009] According to the present invention, it is possible to provide an electrically heated carrier and an exhaust gas purification device that can effectively suppress oxidation of the bonding portion connecting the base layer and the metal electrode. Also, according to the present invention, it is possible to provide an electrically heated carrier and an exhaust gas purification device that can effectively suppress oxidation of the fixing layer that fixes the metal electrode to the electrode layer. [Brief explanation of the drawings]
[0010] [Figure 1] 1 is a schematic cross-sectional view perpendicular to the extension direction of cells of an electrically heated carrier according to an embodiment of the present invention. [Figure 2] 1 is a schematic view showing the appearance of a columnar honeycomb structure and an electrode layer according to an embodiment of the present invention. [Figure 3] 3 is a plan view schematically illustrating an example of the arrangement of a base layer of an electrically heated carrier according to an embodiment of the present invention. FIG. [Figure 4] 1 is a cross-sectional schematic view of a columnar honeycomb structure, an electrode layer, a base layer, a bonding portion, a metal electrode, and an antioxidant layer according to an embodiment of the present invention. [Figure 5]1 is a cross-sectional schematic view of a columnar honeycomb structure, an electrode layer, a base layer, a bonding portion, a metal electrode, and an antioxidant layer according to an embodiment of the present invention. [Figure 6] 1 is a cross-sectional schematic view of a columnar honeycomb structure, an electrode layer, a base layer, a bonding portion, a metal electrode, and an antioxidant layer according to an embodiment of the present invention. [Figure 7] 1 is a cross-sectional schematic view of a columnar honeycomb structure, an electrode layer, a base layer, a bonding portion, a metal electrode, and an antioxidant layer according to an embodiment of the present invention. [Figure 8] 1 is a cross-sectional schematic view of a columnar honeycomb structure, an electrode layer, a base layer, a bonding portion, a metal electrode, and an antioxidant layer according to an embodiment of the present invention. [Figure 9] 1 is a cross-sectional schematic view of a columnar honeycomb structure, an electrode layer, a base layer, a bonding portion, a metal electrode, and an antioxidant layer according to an embodiment of the present invention. [Figure 10] 1 is a cross-sectional schematic view of a columnar honeycomb structure, an electrode layer, a base layer, a bonding portion, a metal electrode, and an antioxidant layer according to an embodiment of the present invention. [Figure 11] 3 is a schematic diagram showing how a base layer of a columnar honeycomb structure and a metal electrode are joined by laser welding or the like in an embodiment of the present invention. FIG. [Figure 12] 1 is a cross-sectional schematic view of a columnar honeycomb structure, an electrode layer, a fixing layer, a metal electrode, and an antioxidant layer according to an embodiment of the present invention. [Figure 13] 1 is a cross-sectional schematic view of a columnar honeycomb structure, an electrode layer, a base layer, a bonding portion, a metal electrode, and an antioxidant layer according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE INVENTION
[0011] Next, embodiments of the present invention will be described in detail with reference to the drawings. It should be understood that the present invention is not limited to the following embodiments, and that appropriate design changes and improvements may be made based on the ordinary knowledge of those skilled in the art without departing from the spirit of the present invention.
[0012] (1. Electrically heated carrier) Fig. 1 is a schematic cross-sectional view perpendicular to the extension direction of cells 18 of an electrically heated carrier 10 according to an embodiment of the present invention. The electrically heated carrier 10 includes a columnar honeycomb structure 11, electrode layers 13a and 13b disposed on the surface of an outer wall 12 of the columnar honeycomb structure 11, a base layer 16 provided on the electrode layers 13a and 13b, metal electrodes 14a and 14b connected to the base layer 16 via bonding regions 20, and an antioxidant layer 21 for protecting the bonding regions 20 from exhaust gas. While Fig. 1 shows a simplified view of the bonding regions 20 and the antioxidant layer 21 for protecting the bonding regions 20 from exhaust gas, the electrically heated carrier 10 according to an embodiment of the present invention may have various configurations, which will be described in detail in each embodiment below with reference to the drawings.
[0013] (1-1. Pillar honeycomb structure) 2 is a schematic view showing the appearance of a pillar-shaped honeycomb structure 11 and electrode layers 13a and 13b according to an embodiment of the present invention. The pillar-shaped honeycomb structure 11 has an outer peripheral wall 12 and partition walls 19 disposed inside the outer peripheral wall 12 to define a plurality of cells 18 that penetrate from one end face to the other end face and form flow paths.
[0014] The outer shape of the pillar-shaped honeycomb structure 11 is not particularly limited as long as it is pillar-shaped, and may be, for example, a pillar with a circular bottom (cylindrical shape), a pillar with an oval bottom, a pillar with a polygonal bottom (quadragonal, pentagonal, hexagonal, heptagonal, octagonal, etc.), etc. The size of the pillar-shaped honeycomb structure 11 is set to a bottom area of 2000 to 20000 mm2 for the purpose of increasing heat resistance (suppressing cracks in the circumferential direction of the outer peripheral wall). 2 It is preferable that the thickness is 5000 to 15000 mm 2 It is more preferable that:
[0015] The columnar honeycomb structure 11 is made of ceramics and has electrical conductivity. As long as the electrically conductive columnar honeycomb structure 11 can generate heat by Joule heat when an electric current is passed through it, there is no particular limitation on the electrical resistivity of the ceramic, but it is preferably 1 to 200 Ωcm, and more preferably 10 to 100 Ωcm. In the present invention, the electrical resistivity of the columnar honeycomb structure 11 is a value measured at 400°C by a four-terminal method.
[0016] The material of the columnar honeycomb structure 11 is not limited, but can be selected from the group consisting of oxide ceramics such as alumina, mullite, zirconia, and cordierite, and non-oxide ceramics such as silicon carbide, silicon nitride, and aluminum nitride. Silicon carbide-metal silicon composites and silicon carbide / graphite composites can also be used. Among these, from the viewpoint of achieving both heat resistance and electrical conductivity, it is preferable that the material of the columnar honeycomb structure 11 contains a silicon-silicon carbide composite or a ceramic containing silicon carbide as the main component. When the material of the columnar honeycomb structure 11 is said to contain a silicon-silicon carbide composite as the main component, it means that the columnar honeycomb structure 11 contains 90 mass% or more of the silicon-silicon carbide composite (total mass) of the entire structure. Here, the silicon-silicon carbide composite material contains silicon carbide particles as aggregate and silicon as a binder that bonds the silicon carbide particles, and it is preferable that a plurality of silicon carbide particles are bonded by the silicon so as to form pores between the silicon carbide particles. When the material of the columnar honeycomb structure 11 is said to be mainly composed of silicon carbide, it means that the columnar honeycomb structure 11 contains silicon carbide (total mass) in an amount of 90 mass% or more of the entire material.
[0017] When the columnar honeycomb structure 11 contains a silicon-silicon carbide composite material, the ratio of the "mass of silicon as a binder" contained in the columnar honeycomb structure 11 to the sum of the "mass of silicon carbide particles as aggregate" contained in the columnar honeycomb structure 11 and the "mass of silicon as a binder" contained in the columnar honeycomb structure 11 is preferably 10 to 40 mass%, and more preferably 15 to 35 mass%. When it is 10 mass% or more, the strength of the columnar honeycomb structure 11 is sufficiently maintained. When it is 40 mass% or less, the shape is more easily maintained during firing.
[0018] Although there are no limitations on the shape of the cells 18 in a cross section perpendicular to the extension direction, a square, a hexagon, an octagon, or a combination thereof is preferred. Among these, a square and a hexagon are preferred. By using such a cell shape, the pressure loss when exhaust gas flows through the columnar honeycomb structure 11 is reduced, and the purification performance of the catalyst is improved. From the viewpoint of easily achieving both structural strength and heating uniformity, a square shape is particularly preferred.
[0019] The thickness of the partition walls 19 that define the cells 18 is preferably 0.1 to 0.3 mm, and more preferably 0.15 to 0.25 mm. When the thickness of the partition walls 19 is 0.1 mm or more, it is possible to prevent a decrease in the strength of the honeycomb structure. When the thickness of the partition walls 19 is 0.3 mm or less, it is possible to prevent an increase in pressure loss when exhaust gas flows through the honeycomb structure when the honeycomb structure is used as a catalyst carrier and a catalyst is loaded thereon. In the present invention, the thickness of the partition walls 19 is defined as the length of a portion that passes through the partition walls 19, of a line segment connecting the centers of gravity of adjacent cells 18 in a cross section perpendicular to the extension direction of the cells 18.
[0020] The columnar honeycomb structure 11 has a cell density of 40 to 150 cells / cm in a cross section perpendicular to the flow path direction of the cells 18. 2 It is preferable that the number of cells is 70 to 100. 2By setting the cell density in this range, it is possible to increase the purification performance of the catalyst while minimizing the pressure loss when exhaust gas flows through it. 2 If the cell density is 150 cells / cm or more, a sufficient catalyst carrying area is ensured. 2 When the columnar honeycomb structure 11 is used as a catalyst carrier to support a catalyst, excessive pressure loss during the flow of exhaust gas is suppressed if the cell density is equal to or less than this value. The cell density is a value obtained by dividing the number of cells by the area of one bottom surface portion of the columnar honeycomb structure 11 excluding the outer wall 12 portion.
[0021] Providing the outer peripheral wall 12 of the columnar honeycomb structure 11 is useful from the viewpoint of ensuring the structural strength of the columnar honeycomb structure 11 and suppressing leakage of the fluid flowing through the cells 18 from the outer peripheral wall 12. Specifically, the thickness of the outer peripheral wall 12 is preferably 0.1 mm or more, more preferably 0.15 mm or more, and even more preferably 0.2 mm or more. However, if the outer peripheral wall 12 is made too thick, the strength becomes too high, which disrupts the strength balance with the partition walls 19 and reduces thermal shock resistance. Therefore, the thickness of the outer peripheral wall 12 is preferably 1.0 mm or less, more preferably 0.7 mm or less, and even more preferably 0.5 mm or less. Here, the thickness of the outer peripheral wall 12 is defined as the thickness in the direction normal to the tangent of the outer peripheral wall 12 at the measurement point when the portion of the outer peripheral wall 12 where the thickness is to be measured is observed in a cross section perpendicular to the extension direction of the cells.
[0022] The partition walls 19 can be porous. The porosity of the partition walls 19 is preferably 35 to 60%, and more preferably 35 to 45%. When the porosity is 35% or more, deformation during firing is more easily suppressed. When the porosity is 60% or less, the strength of the honeycomb structure is sufficiently maintained. The porosity is a value measured by a mercury porosimeter.
[0023] The average pore diameter of the partition walls 19 of the columnar honeycomb structure 11 is preferably 2 to 15 μm, and more preferably 4 to 8 μm. When the average pore diameter is 2 μm or more, the electrical resistivity is prevented from becoming too high. When the average pore diameter is 15 μm or less, the electrical resistivity is prevented from becoming too low. The average pore diameter is a value measured by a mercury porosimeter.
[0024] (1-2. Electrode layer) Electrode layers 13a and 13b are disposed on the surface of the outer wall 12 of the columnar honeycomb structure 11. The electrode layers 13a and 13b may be a pair of electrode layers 13a and 13b disposed opposite each other across the central axis of the columnar honeycomb structure 11.
[0025] Although there are no particular restrictions on the formation regions of the electrode layers 13a, 13b, from the viewpoint of improving the uniform heat generation property of the columnar honeycomb structure 11, it is preferable that each of the electrode layers 13a, 13b extend in a strip shape on the outer surface of the outer peripheral wall 12 in the circumferential direction of the outer peripheral wall 12 and in the extension direction of the cells. Specifically, it is desirable that each of the electrode layers 13a, 13b extend over 80% or more of the length between both bottom surfaces of the columnar honeycomb structure 11, preferably over 90% or more of the length, and more preferably over the entire length, from the viewpoint of facilitating the spread of current in the axial direction of the electrode layers 13a, 13b.
[0026] The thickness of each electrode layer 13a, 13b is preferably 0.01 to 5 mm, and more preferably 0.01 to 3 mm. Setting the thickness within this range can improve uniform heat generation. When the thickness of each electrode layer 13a, 13b is 0.01 mm or more, electrical resistance is appropriately controlled, allowing for more uniform heat generation. When the thickness is 5 mm or less, the risk of breakage during canning is reduced. The thickness of each electrode layer 13a, 13b is defined as the thickness in the direction normal to the tangent at the measurement point on the outer surface of each electrode layer 13a, 13b when the location of the electrode layer 13a, 13b where the thickness is to be measured is observed in a cross section perpendicular to the extension direction of the cell.
[0027] By making the electrical resistivity of each electrode layer 13a, 13b lower than that of the columnar honeycomb structure 11, electricity flows preferentially through the electrode layers 13a, 13b, and electricity spreads more easily in the flow path direction and circumferential direction of the cell when current is applied. The electrical resistivity of the electrode layers 13a, 13b is preferably 1 / 10 or less, more preferably 1 / 20 or less, and even more preferably 1 / 30 or less of the electrical resistivity of the columnar honeycomb structure 11. However, if the difference in electrical resistivity between the two is too large, current will concentrate between the ends of the opposing electrode layers 13a, 13b, causing uneven heat generation in the columnar honeycomb structure. Therefore, the electrical resistivity of the electrode layers 13a, 13b is preferably 1 / 200 or more, more preferably 1 / 150 or more, and even more preferably 1 / 100 or more of the electrical resistivity of the columnar honeycomb structure 11. In the present invention, the electrical resistivity of the electrode layers 13a and 13b is a value measured at 400°C by a four-terminal method.
[0028] The material of each electrode layer 13a, 13b can be a metal, a conductive ceramic, or a composite (cermet) of a metal and a conductive ceramic. Examples of metals include, for example, a single metal such as Cr, Fe, Co, Ni, Si, or Ti, or an alloy containing at least one metal selected from the group consisting of these metals. Examples of conductive ceramics include, but are not limited to, silicon carbide (SiC) and metal compounds such as metal silicides, such as tantalum silicide (TaSi2) and chromium silicide (CrSi2). Specific examples of composites (cermets) of a metal and a conductive ceramic include composites of metal silicon and silicon carbide, composites of metal silicides, such as tantalum silicide or chromium silicide, and metal silicon and silicon carbide, as well as composites of one or more of the above metals to which one or more insulating ceramics, such as alumina, mullite, zirconia, cordierite, silicon nitride, and aluminum nitride, have been added to reduce thermal expansion. As the material for the electrode layers 13a, 13b, among the various metals and conductive ceramics mentioned above, a combination of a metal silicide such as tantalum silicide or chromium silicide with a composite material of metal silicon and silicon carbide is preferred because it can be fired simultaneously with the columnar honeycomb structure portion, which simplifies the manufacturing process.
[0029] (1-3. Base layer) In the electrically heated carrier 10 according to the embodiment of the present invention, a base layer 16 is provided on the electrode layers 13a and 13b. The base layer 16 can be formed on the surfaces of the electrode layers 13a and 13b and is generally flat (specifically, curved so as to fit along the outer surfaces of the electrode layers 13a and 13b). The base layer 16 is electrically conductive. The base layer 16 may have a thermal expansion coefficient between that of the electrode layers 13a and 13b (the linear expansion coefficient of the electrode layers 13a and 13b is relatively small) and that of the metal electrodes 14a and 14b (the linear expansion coefficient of the metal electrodes 14a and 14b is relatively large). In this case, the base layer 16 has the function of absorbing the difference in thermal expansion between the electrode layers 13a and 13b and the metal electrodes 14a and 14b.
[0030] The underlayer 16 can be made of a conductive ceramic. Ceramics constituting the underlayer 16 include, but are not limited to, silicon carbide (SiC), metal compounds such as metal silicides, such as tantalum silicide (TaSi2) and chromium silicide (CrSi2), and composites (cermets) consisting of a combination of one or more ceramics and one or more metals. Specific examples of cermets include composites of metal silicon and silicon carbide, composites of metal silicides, such as tantalum silicide or chromium silicide, and metal silicon and silicon carbide, as well as composites in which one or more insulating ceramics, such as alumina, mullite, zirconia, cordierite, silicon nitride, and aluminum nitride, are added to one or more of the above metals to reduce thermal expansion.
[0031] The number and arrangement of the base layers 16 are not limited and can be set as appropriate within the range necessary to fix the metal electrodes 14a and 14b. The base layers 16 can be formed into any shape, such as a circle, an ellipse, or a polygon, in a plan view. From the viewpoints of productivity and practicality, the shape of the base layers 16 is preferably a circle or a rectangle.
[0032] (1-4. Metal electrode) The metal electrodes 14a, 14b are connected to the base layer 16 by a bonding portion 20. The metal electrodes 14a, 14b may be a pair of metal electrodes arranged such that one metal electrode 14a faces the other metal electrode 14b across the central axis of the columnar honeycomb structure 11. When a voltage is applied via the electrode layers 13a, 13b, the metal electrodes 14a, 14b are energized and can generate heat in the columnar honeycomb structure 11 by Joule heat. Therefore, the electrically heated carrier 10 can also be suitably used as a heater. The applied voltage is preferably 12 to 900 V, more preferably 64 to 600 V, but the applied voltage can be changed as appropriate.
[0033] The material of the metal electrodes 14a, 14b is not particularly limited as long as it is a metal, and simple metals and alloys can be used, but from the viewpoints of corrosion resistance, electrical resistivity, and linear expansion coefficient, an alloy containing at least one selected from the group consisting of Cr, Fe, Co, Ni, and Ti is preferable, and stainless steel and an Fe-Ni alloy are more preferable. The shape and size of the metal electrodes 14a, 14b are not particularly limited, and can be designed appropriately depending on the size, electrical conductivity, etc. of the electrically heated carrier 10.
[0034] The metal electrodes 14a, 14b may have two or more electrode portions 15. Each electrode portion 15 may be fixed to the outer surface of the base layer 16. Here, the electrode portions 15 may be fixed to the base layer 16 by welding, or may be fixed to the electrode layers 13a, 13b by a fixing layer formed by thermal spraying.
[0035] 3, each of the metal electrodes 14a and 14b has three comb-shaped electrode portions 15, and each of the electrode portions 15 is fixed to two base layers 16. In this manner, electrical connection between the comb-shaped electrode portions 15 and the electrode layers 13a and 13b may be achieved by two or more base layers 16 spaced apart from each other.
[0036] Although the electrode portion 15 is shaped like a comb in FIG. 3, any shape can be adopted as long as it can be fixed to the base layer 16 and electrically connected to the electrode layers 13a and 13b, or as long as it can be fixed to the electrode layers 13a and 13b by thermal spraying.
[0037] (1-5. Antioxidant layer) The electrically heated carrier 10 in the embodiment of the present invention is provided with an antioxidant layer 21 for protecting the bonded portion 20 from exhaust gas. In the present invention, the bonded portion 20 and the antioxidant layer 21 that protects the bonded portion 20 may have various configurations. Each embodiment will be described in detail below with reference to the drawings.
[0038] [Embodiment 1] Fig. 4 shows a cross-sectional schematic diagram of the columnar honeycomb structure 11, electrode layers 13a and 13b, base layer 16, bonding portion 20, metal electrodes 14a and 14b, and antioxidant layer 21a in embodiment 1 of the present invention. In embodiment 1 shown in Fig. 4, a second base layer or second electrode layer 17 for further reducing thermal stress is provided between the electrode layers 13a and 13b and base layer 16. The second base layer or second electrode layer 17 does not need to be provided, or a third layer for further reducing thermal stress may be provided on the second base layer or second electrode layer 17.
[0039] The joints 20 connecting the base layer 16 and the metal electrodes 14a, 14b are formed between the base layer 16 and the metal electrodes 14a, 14b by, for example, performing laser welding or the like from the metal electrodes 14a, 14b side with the metal electrodes 14a, 14b provided on the base layer 16, melting a portion of the metal electrodes 14a, 14b. The example shown in FIG. 4 schematically illustrates a configuration in which three columnar joints 20 are provided at intervals between the base layer 16 and the metal electrodes 14a, 14b. The joints 20 of this type can be formed, for example, by performing laser spot welding from the metal electrodes 14a, 14b side with the metal electrodes 14a, 14b provided on the base layer 16. The size, shape, number, and the like of the joints 20 are not particularly limited.
[0040] The antioxidant layer 21a of the columnar honeycomb structure 11 in the first embodiment of the present invention is provided continuously from the side surfaces of the metal electrodes 14a, 14b to the base layer 16, sealing the gaps 22, and further to the surfaces of the electrode layers 13a, 13b, as in the example of Fig. 4. The antioxidant layer 21a is not limited to this, and may be provided from the side surfaces of the metal electrodes 14a, 14b to partway along the side surfaces of the base layer 16, sealing the gaps 22, as shown in Fig. 5. In this way, the antioxidant layer 21a may have any form as long as it is provided so as to seal the gaps 22 between the base layer 16 and the metal electrodes 14a, 14b.
[0041] Furthermore, when the metal electrodes 14a, 14b are provided on the base layer 16 and ultrasonic welding is performed from the metal electrodes 14a, 14b side to connect the base layer 16 and the metal electrodes 14a, 14b, a bonded portion 20a is formed over the entire surface between the base layer 16 and the metal electrodes 14a, 14b, as shown in Fig. 6. In this case as well, the antioxidant layer 21a is provided so as to seal the gap 22 between the base layer 16 and the metal electrodes 14a, 14b.
[0042] The portion of the antioxidant layer 21a that seals the gap 22 between the base layer 16 and the metal electrodes 14a, 14b is particularly susceptible to load due to thermal expansion of the metal electrodes 14a, 14b. Therefore, to increase the strength and prevent cracks from occurring, it is preferable to form the antioxidant layer 21a with a thickness of 10 μm or more. Furthermore, the thickness of the antioxidant layer 21a is more preferably 10 to 100 μm.
[0043] The anti-oxidation layer 21a of the columnar honeycomb structure 11 in the first embodiment of the present invention is provided from the outer surfaces of the electrode layers 13a, 13b to the outer surfaces of the metal electrodes 14a, 14b so as to seal the gaps 22 between the base layer 16 and the metal electrodes 14a, 14b. Here, the gaps 22 between the base layer 16 and the metal electrodes 14a, 14b are gaps of, for example, about several tens of μm between the base layer 16 and the metal electrodes 14a, 14b. In general, the bonded portions 20, 20a may be oxidized by being exposed to exhaust gases diffusing from the gaps 22 between the base layer 16 and the metal electrodes 14a, 14b. In contrast, in the columnar honeycomb structure 11 according to the first embodiment of the present invention, the antioxidant layer 21a is provided from the outer surfaces of the electrode layers 13a, 13b to the outer surfaces of the metal electrodes 14a, 14b so as to seal the gaps 22 between the base layer 16 and the metal electrodes 14a, 14b. This prevents exhaust gas from entering through the gaps 22, thereby effectively preventing oxidation of the bonded portions 20, 20a.
[0044] The material for the antioxidant layer 21a can be ceramic, glass, or a composite material of ceramic and glass. The composite material can be, for example, a material containing 50 volume % or more, more preferably 60 volume % or more, and even more preferably 70 volume % or more of glass. Examples of ceramics that can be used to form the antioxidant layer 21a include SiO2-based, Al2O3-based, SiO2-Al2O3-based, SiO2-ZrO2-based, and SiO2-Al2O3-ZrO2-based ceramics. Examples of the glass that constitutes the antioxidant layer 21a include lead-free B2O3-Bi2O3-based, B2O3-ZnO-Bi2O3-based, B2O3-ZnO-based, V2O5-P2O5-based, SnO-P2O5-based, SnO-ZnO-P2O5-based, SiO2-B2O3-Bi2O3-based, SiO2-Bi2O3-Na2O-based, and SiO2-Al2O3-MgO-based glasses.
[0045] [Embodiment 2] FIG. 7 is a cross-sectional schematic diagram showing the columnar honeycomb structure 11, the electrode layers 13a and 13b, the base layer 16, the bonding portion 20, the metal electrodes 14a and 14b, and the antioxidant layer 21b according to the second embodiment of the present invention.
[0046] The antioxidant layer 21b of the columnar honeycomb structure 11 in the second embodiment of the present invention is provided on the surface of the joint portion 20. By providing the antioxidant layer 21b on the surface of the joint portion 20 in this manner, it is possible to prevent the joint portion 20 from being exposed to exhaust gas. As a result, it is possible to effectively prevent oxidation of the joint portion 20. Furthermore, with this configuration, since the antioxidant layer 21b is provided on the surface of the joint portion 20, it is possible to reduce thermal stress on the antioxidant layer 21b due to thermal expansion of the metal electrodes 14a, 14b, etc. As a result, it is possible to effectively prevent cracks from occurring.
[0047] In the example shown in Fig. 7, the antioxidant layer 21b is provided so as to fill the space from the surface of the joint portion 20 to the ends of the metal electrodes 14a, 14b, but this is not limiting. For example, as shown in Fig. 8, the antioxidant layer 21b may be provided so as to fill the space from the surface of the joint portion 20 to partway to the ends of the metal electrodes 14a, 14b. The antioxidant layer 21b can be formed using the same material as the antioxidant layer 21a shown in the first embodiment of the present invention. Alternatively, the joint portion 20 may be a joint portion 20a formed by ultrasonic welding, as shown in Fig. 6.
[0048] [Embodiment 3] FIG. 9 is a cross-sectional schematic diagram showing the columnar honeycomb structure 11, the electrode layers 13a and 13b, the base layer 16, the bonding portion 20, the metal electrodes 14a and 14b, and the antioxidant layer 21c according to the third embodiment of the present invention.
[0049] The antioxidant layer 21c of the columnar honeycomb structure 11 in the third embodiment of the present invention is provided between the base layer 16 and the metal electrodes 14a, 14b, spaced apart from the bonded portions 20. By providing the antioxidant layer 21c between the base layer 16 and the metal electrodes 14a, 14b, spaced apart from the bonded portions 20, the bonded portions 20 can be prevented from being exposed to exhaust gas. As a result, oxidation of the bonded portions 20 can be effectively prevented. Furthermore, with this configuration, the antioxidant layer 21c is provided between the base layer 16 and the metal electrodes 14a, 14b, so that thermal stress on the antioxidant layer 21c due to thermal expansion of the metal electrodes 14a, 14b can be reduced. As a result, the occurrence of cracks can be effectively prevented.
[0050] The antioxidant layer 21c can be formed using the same material as the antioxidant layer 21a described in embodiment 1 of the present invention. The bonding portion 20 may be a bonding portion 20a formed by ultrasonic welding, as shown in FIG.
[0051] [Embodiment 4] FIG. 10 is a cross-sectional schematic diagram showing the columnar honeycomb structure 11, the electrode layers 13a and 13b, the base layer 16, the bonded portion 20b, the metal electrodes 14a and 14b, and the antioxidant layer 21d according to the fourth embodiment of the present invention.
[0052] The antioxidant layer 21d of the columnar honeycomb structure 11 in the fourth embodiment of the present invention is filled between the base layer 16 and the metal electrodes 14a, 14b. By filling the antioxidant layer 21d between the base layer 16 and the metal electrodes 14a, 14b in this manner, it is possible to prevent the joint portion 20b from being exposed to exhaust gas. As a result, it is possible to effectively prevent oxidation of the joint portion 20b. Furthermore, with this configuration, since the antioxidant layer 21d is provided between the base layer 16 and the metal electrodes 14a, 14b, it is possible to reduce thermal stress on the antioxidant layer 21d due to thermal expansion of the metal electrodes 14a, 14b, etc. As a result, it is possible to effectively prevent cracks from occurring.
[0053] FIG. 11 is a schematic diagram illustrating the joining of the base layer 16 and the metal electrodes 14a, 14b of the columnar honeycomb structure 11 according to the fourth embodiment of the present invention by laser welding or the like. As shown in the upper diagram of FIG. 11, first, a coating layer 23 made of an antioxidant layer-forming material is provided on the base layer 16. Next, the metal electrodes 14a, 14b are placed on the coating layer 23. Next, spot welding is performed on the metal electrodes 14a, 14b by laser welding or the like. At this time, the application of energy by laser welding or the like melts the metal electrodes 14a, 14b, forming a mixture with the antioxidant layer-forming material of the underlying coating layer 23. This mixture forms the joining region 20b. The antioxidant layer-forming material constituting the coating layer 23 can be formed using the same material as the antioxidant layer 21a described in the first embodiment of the present invention. Therefore, the joining region 20b is a mixture of metal and an inorganic material such as glass.
[0054] Furthermore, by forming the bonding areas 20b as shown in FIG. 11, even if there are tiny pores between the bonding areas 20b, the pores are filled with the antioxidant layer-forming material, thereby further improving the oxidation resistance of the bonding areas 20b.
[0055] [Embodiment 5] FIG. 12 is a cross-sectional schematic diagram showing the columnar honeycomb structure 11, electrode layers 13a and 13b, fixing layer 24, metal electrodes 14a and 14b, and antioxidant layer 21e of the electrically heated carrier according to the fifth embodiment of the present invention.
[0056] In the electrically heated carrier according to the fifth embodiment of the present invention, electrode layers 13a and 13b are disposed on the surface of the outer wall of the columnar honeycomb structure 11 shown in the first embodiment, and metal electrodes 14a and 14b are provided on the electrode layers 13a and 13b. A fixing layer 24 is provided so as to cover the metal electrodes 14a and 14b, and an antioxidant layer 21e is provided so as to cover the fixing layer 24. The fixing layer 24 fixes the metal electrodes 14a and 14b to the electrode layers 13a and 13b.
[0057] In this way, by providing the fixing layer 24 so as to cover the metal electrodes 14a, 14b and further providing the antioxidant layer 21e so as to cover the fixing layer 24, it is possible to prevent the fixing layer 24, which serves as a joining portion, from being exposed to exhaust gas. As a result, oxidation of the fixing layer 24 can be effectively prevented. Furthermore, with this configuration, the antioxidant layer 21e is provided on the fixing layer 24 that covers the metal electrodes 14a, 14b, so it is possible to reduce thermal stress on the antioxidant layer 21e due to thermal expansion of the metal electrodes 14a, 14b, etc. As a result, it is possible to effectively prevent cracks from occurring.
[0058] The fixing layer 24 in the fifth embodiment can be formed by, for example, thermal spraying. After the metal electrodes 14a, 14b are provided on the electrode layers 13a, 13b, a material such as a mixed spray material of NiCrAlY and mullite is sprayed onto the metal electrodes 14a, 14b by thermal spraying, thereby forming the fixing layer 24. Alternatively, the antioxidant layer 21e can be formed so as to cover the fixing layer 24 using the same material as the antioxidant layer 21a described in the first embodiment of the present invention.
[0059] [Embodiment 6] Figures 13(a), 13(b), 13(c) and 13(d) show cross-sectional schematic diagrams of the columnar honeycomb structure 11, electrode layers 13a, 13b, second base layer or electrode layer 17, base layer 16, bonding portion 20d, metal electrodes 14a, 14b and antioxidant layers 21f, 21g, 21h, 21i of an electrically heated carrier in embodiment 6 of the present invention.
[0060] In the electrically heated carrier according to the fifth embodiment of the present invention, electrode layers 13a and 13b are disposed on the surface of the outer wall of the columnar honeycomb structure 11 shown in the first embodiment, and a second base layer or electrode layer 17 and a base layer 16 are provided on the electrode layers 13a and 13b. The base layer 16 is joined to the metal electrodes 14a and 14b at joint portions 20d by brazing the metal electrodes 14a and 14b.
[0061] In the embodiment shown in Figure 13(a), an antioxidant layer 21f is provided continuously from the side surfaces of the metal electrodes 14a, 14b to the outer surfaces of the electrode layers 13a, 13b, and is configured to seal the gap between the base layer 16 and the metal electrodes 14a, 14b. In the embodiment shown in Figure 13(b), an antioxidant layer 21g is provided continuously from the bottom surfaces of the metal electrodes 14a, 14b to the outer surfaces of the electrode layers 13a, 13b, and is configured to seal the gap between the base layer 16 and the metal electrodes 14a, 14b. In the embodiment shown in Figure 13(c), a gap without a bonding portion 20d is provided between the metal electrodes 14a, 14b and the base layer 16, and an antioxidant layer 21h is provided in the gap so as to contact the bonding portion 20d. In the embodiment shown in FIG. 13(d), a gap having no bonding portion 20d is provided between the metal electrodes 14a, 14b and the underlayer 16, and an antioxidant layer 21i is provided in the gap, spaced apart from the bonding portion 20d.
[0062] 13(a), 13(b), 13(c), and 13(d), the provision of the antioxidant layers 21f, 21g, 21h, and 21i can prevent the bonding portion 20d from being exposed to exhaust gas, thereby effectively preventing oxidation of the bonding portion 20d.
[0063] By supporting a catalyst on the electrically heated support 10, the electrically heated support 10 can be used as a catalyst body. A fluid such as automobile exhaust gas can be passed through the flow paths of the multiple cells 18. Examples of the catalyst include precious metal catalysts and other catalysts. Precious metal catalysts include three-way catalysts and oxidation catalysts in which a precious metal such as platinum (Pt), palladium (Pd), or rhodium (Rh) is supported on the surface of alumina pores and a promoter such as ceria or zirconia is included, or alkaline earth metals and platinum are used to convert nitrogen oxides (NO x ) as a storage component of NO x Examples of catalysts that do not use precious metals include NOx storage reduction catalysts (LNT catalysts) containing copper-substituted or iron-substituted zeolites. xExamples include selective catalytic reduction catalysts (SCR catalysts). Two or more catalysts selected from the group consisting of these catalysts may be used. There are no particular limitations on the method for supporting the catalyst, and the method can be carried out in accordance with the conventional method for supporting a catalyst on a honeycomb structure.
[0064] (2. Manufacturing method of electrically heated carrier) Next, a method for manufacturing the electrically heated carrier 10 according to the present invention will be described by way of example. In one embodiment, the method for manufacturing the electrically heated carrier 10 according to the present invention includes a step A1 of obtaining an unfired honeycomb structure part with an electrode layer forming paste, a step A2 of firing the unfired honeycomb structure part with the electrode layer forming paste to obtain a columnar honeycomb structure, and a step A3 of welding metal electrodes to the columnar honeycomb structure.
[0065] Step A1 is a step of preparing a honeycomb formed body, which is a precursor of a honeycomb structure part, and applying an electrode layer forming paste to the side surface of the honeycomb formed body to obtain an unfired honeycomb structure part with the electrode layer forming paste. The honeycomb formed body can be prepared in accordance with a method for preparing a honeycomb formed body in a known method for manufacturing a honeycomb structure part. For example, first, a forming raw material is prepared by adding metal silicon powder (metal silicon), a binder, a surfactant, a pore-forming material, water, etc. to silicon carbide powder (silicon carbide). It is preferable that the mass of metal silicon is 10 to 40 mass% with respect to the total mass of the silicon carbide powder and the metal silicon. The average particle diameter of the silicon carbide particles in the silicon carbide powder is preferably 3 to 50 μm, more preferably 3 to 40 μm. The average particle diameter of the metal silicon (metal silicon powder) is preferably 2 to 35 μm. The average particle diameters of silicon carbide particles and metallic silicon (metallic silicon particles) refer to the arithmetic mean diameters based on volume when the particle size frequency distribution is measured by laser diffraction. Silicon carbide particles are fine particles of silicon carbide that make up silicon carbide powder, and metallic silicon particles are fine particles of metallic silicon that make up metallic silicon powder. Note that this is the blend of the molding raw materials when the material of the honeycomb structure is a silicon-silicon carbide composite material; when the material of the honeycomb structure is silicon carbide, metallic silicon is not added.
[0066] Examples of binders include methyl cellulose, hydroxypropyl methyl cellulose, hydroxypropoxyl cellulose, hydroxyethyl cellulose, carboxymethyl cellulose, polyvinyl alcohol, etc. Among these, it is preferable to use methyl cellulose and hydroxypropoxyl cellulose in combination. The content of the binder is preferably 2.0 to 10.0 parts by mass when the total mass of the silicon carbide powder and the metallic silicon powder is 100 parts by mass.
[0067] The content of water is preferably 20 to 60 parts by mass when the total mass of the silicon carbide powder and the metallic silicon powder is taken as 100 parts by mass.
[0068] Examples of surfactants that can be used include ethylene glycol, dextrin, fatty acid soap, and polyalcohol. These may be used alone or in combination of two or more. The content of the surfactant is preferably 0.1 to 2.0 parts by mass when the total mass of the silicon carbide powder and the metallic silicon powder is 100 parts by mass.
[0069] The pore-forming material is not particularly limited as long as it forms pores after firing, and examples include graphite, starch, foamed resin, water-absorbent resin, silica gel, etc. The content of the pore-forming material is preferably 0.5 to 10.0 parts by mass when the total mass of the silicon carbide powder and metallic silicon powder is 100 parts by mass. The average particle diameter of the pore-forming material is preferably 10 to 30 μm. If it is smaller than 10 μm, pores may not be sufficiently formed. If it is larger than 30 μm, clogging of the die may occur during molding. The average particle diameter of the pore-forming material refers to the arithmetic mean diameter on a volume basis when the particle size frequency distribution is measured by laser diffraction. When the pore-forming material is a water-absorbent resin, the average particle diameter of the pore-forming material refers to the average particle diameter after water absorption.
[0070] Next, the obtained molding raw materials are kneaded to form a clay, and the clay is then extruded to produce a honeycomb molded body. During extrusion molding, a die having the desired overall shape, cell shape, partition wall thickness, cell density, etc. can be used. Next, it is preferable to dry the obtained honeycomb molded body. If the length of the honeycomb molded body in the central axis direction is not the desired length, both bottom portions of the honeycomb molded body can be cut to the desired length. The honeycomb molded body after drying is called a dried honeycomb body.
[0071] Next, an electrode layer forming paste for forming the electrode layer is prepared. The electrode layer forming paste can be formed by adding various additives appropriately to raw material powders (metal powder, ceramic powder, etc.) formulated according to the required characteristics of the electrode layer and kneading them. When the electrode layer has a laminated structure, the bonding strength between the metal terminal and the electrode layer tends to be improved by making the average particle diameter of the metal powder in the paste for the second electrode layer larger than the average particle diameter of the metal powder in the paste for the first electrode layer. The average particle diameter of the metal powder refers to the arithmetic mean diameter on a volume basis when measuring the particle size frequency distribution using laser diffraction.
[0072] Next, the obtained electrode layer forming paste is applied to the side surface of a honeycomb formed body (typically a dried honeycomb body) to obtain an unfired honeycomb structure part with the electrode layer forming paste. The method of preparing the electrode layer forming paste and the method of applying the electrode layer forming paste to the honeycomb formed body can be performed in accordance with known methods for manufacturing honeycomb structures, but in order to make the electrode layer have a lower electrical resistivity than the honeycomb structure part, the metal content ratio can be made higher than that of the honeycomb structure part, or the particle size of the metal particles can be made smaller.
[0073] As a modified example of the manufacturing method of the pillar-shaped honeycomb structure, the honeycomb formed body may be fired once before applying the electrode layer forming paste in step A1. That is, in this modified example, the honeycomb formed body is fired to prepare a honeycomb fired body, and the electrode layer forming paste is applied to the honeycomb fired body.
[0074] In step A2, the unfired honeycomb structure part with the electrode layer forming paste is fired to obtain a columnar honeycomb structure. Before firing, the unfired honeycomb structure part with the electrode layer forming paste may be dried. Furthermore, before firing, degreasing may be performed to remove binders and the like. As firing conditions, heating at 1400 to 1500°C for 1 to 20 hours in an inert atmosphere such as nitrogen or argon is preferred. Furthermore, after firing, oxidation treatment is preferably performed at 1200 to 1350°C for 1 to 10 hours to improve durability. The degreasing and firing methods are not particularly limited, and firing can be performed using an electric furnace, a gas furnace, or the like.
[0075] In step A3, a conductive material paste for forming a base layer is applied to the surface of the electrode layer on the columnar honeycomb structure. The conductive material paste prepared in this manner is applied in a predetermined arrangement using a curved surface printing machine or the like, dried, and then fired to form the base layer. To prepare the conductive material paste, first, a ceramic raw material is prepared by mixing metal powder (metal powder such as NiCr-based material or stainless steel) and oxide powder (oxide powder such as Cd, alumina, or mullite) in a volume ratio of 20 to 85% by volume of metal and 15 to 80% by volume of oxide powder. Next, 1 mass% of binder, 1 mass% of surfactant, and 20 to 40 mass% of water are added to the ceramic raw material to prepare a base layer forming paste. Alternatively, the base layer may be formed in a predetermined arrangement and shape by thermal spraying the conductive material.
[0076] Next, metal electrodes are fixed onto the base layer by welding. The welding method will be described in detail below. First, comb-shaped electrodes are placed on the honeycomb structure on which the base layer has been formed, and laser welding or ultrasonic welding is performed on the areas where each comb-shaped electrode overlaps the base layer. The laser spot diameter when performing laser welding can be in the range of 0.5 to 3.0 mm. The vibration frequency when performing ultrasonic welding can be in the range of 20 kHz to 40 kHz, and the pressure can be in the range of 10 N to 30 N.
[0077] At this time, by performing a plurality of spot welding by laser welding, it is possible to form a joint 20 as shown in Fig. 4. Furthermore, by performing ultrasonic welding, it is possible to form a joint 20a as shown in Fig. 6.
[0078] Next, an antioxidant layer is provided from the outer surface of the base layer to the outer surface of the metal electrode so as to seal the gap between the base layer and the metal electrode, thereby forming the antioxidant layer 21a as shown in Figures 4 to 6. In this case, after joining the base layer and the metal electrode, an antioxidant is sprayed onto them using a spray or the like, and then baked preferably in a vacuum atmosphere at 800 to 1100°C for 4 to 8 hours, thereby forming the antioxidant layer 21a.
[0079] 7 to 9, a plurality of spot welds can be formed by laser welding, and then antioxidant layers 21b and 21c can be formed as shown in Figs. 7 to 9. In this case, an antioxidant is applied to the portions of the base layer other than the bonding portions, and after bonding the metal electrodes by a method such as laser welding, the resulting product is fired at 800 to 1100°C for 4 to 8 hours, preferably in a vacuum atmosphere, to form antioxidant layers 21b and 21c.
[0080] Furthermore, as shown in Figure 11, by providing a coating layer made of an antioxidant layer-forming material between the base layer and the metal electrode and then performing laser welding from the metal electrode side, an antioxidant layer 21d as shown in Figure 10 can be formed.
[0081] (3. Exhaust gas purification device) The electrically heated carrier according to the embodiment of the present invention described above can be used in an exhaust gas purification device. The exhaust gas purification device includes an electrically heated carrier and a can body that holds the electrically heated carrier. In the exhaust gas purification device, the electrically heated carrier is installed midway through an exhaust gas flow path for flowing exhaust gas from an engine. The can body can be a metallic cylindrical member or the like that houses the electrically heated carrier. [Example]
[0082] The following examples are provided to provide a better understanding of the present invention and its advantages, but the present invention is not limited to these examples.
[0083] Example 1 (1. Making cylindrical clay) A ceramic raw material was prepared by mixing silicon carbide (SiC) powder and metallic silicon (Si) powder in an 80:20 mass ratio. Hydroxypropyl methylcellulose as a binder, a water-absorbent resin as a pore-forming material, and water were added to the ceramic raw material to form a molding raw material. The molding raw material was then kneaded using a vacuum kneader to produce a cylindrical clay. The binder content was 7 parts by mass per 100 parts by mass of the silicon carbide (SiC) powder and metallic silicon (Si) powder. The pore-forming material content was 3 parts by mass per 100 parts by mass of the silicon carbide (SiC) powder and metallic silicon (Si) powder. The water content was 42 parts by mass per 100 parts by mass of the silicon carbide (SiC) powder and metallic silicon (Si) powder. The average particle size of the silicon carbide powder was 20 μm, and the average particle size of the metallic silicon powder was 6 μm. The average particle size of the pore-forming material was 20 μm. The average particle sizes of the silicon carbide powder, the metallic silicon powder, and the pore-forming material refer to the arithmetic mean diameter on a volume basis when the particle size frequency distribution was measured by laser diffraction.
[0084] (2. Preparation of dried honeycomb body) The obtained cylindrical clay was molded using an extruder with a checkerboard die structure to obtain a cylindrical honeycomb molded body in which each cell shape in the cross section perpendicular to the cell flow direction is square. This honeycomb molded body was dried by high-frequency dielectric heating, and then dried at 120°C for 2 hours using a hot air dryer. Both bottom surfaces were cut to a predetermined length to produce a dried honeycomb body.
[0085] (3. Preparation of electrode layer forming paste) An electrode layer forming paste was prepared by mixing metal silicon (Si) powder, silicon carbide (SiC) powder, methyl cellulose, glycerin, and water using a planetary centrifugal mixer. The Si powder and SiC powder were blended in a volume ratio of Si powder:SiC powder = 40:60. Furthermore, when the total of the Si powder and SiC powder was 100 parts by mass, the amount of methyl cellulose was 0.5 parts by mass, the amount of glycerin was 10 parts by mass, and the amount of water was 38 parts by mass. The average particle diameter of the metal silicon powder was 6 μm. The average particle diameter of the silicon carbide powder was 35 μm. These average particle diameters refer to the arithmetic mean diameters based on volume when the particle size frequency distribution was measured by laser diffraction.
[0086] (4. Application and firing of electrode layer forming paste) Next, this electrode layer forming paste was applied to the dried honeycomb body with an appropriate area and film thickness using a curved surface printing machine, and then dried at 120°C for 30 minutes in a hot air dryer.After that, it was fired together with the dried honeycomb body at 1400°C in an Ar atmosphere for 3 hours to form a columnar honeycomb structure.
[0087] (5. Preparation of Undercoat Layer Forming Paste) A ceramic raw material was prepared by mixing metal powder (NiCr-based materials, stainless steel, etc.) and oxide powder (Cd, alumina, mullite, etc.) in a volume ratio of 20-85% metal and 15-80% oxide powder. A paste raw material was prepared by adding 1 mass% binder, 1 mass% surfactant, and 20-40 mass% water to this ceramic raw material. The average particle size of the metal powder measured by laser diffraction was 10 μm, and the average particle size of the oxide powder was 5 μm.
[0088] (6. Application and firing of base layer forming paste) The above-mentioned base layer forming paste was applied to the electrode layer of the columnar honeycomb structure by a curved surface printing machine, and then dried in a hot air dryer at 120°C for 30 minutes, and then fired in an Ar atmosphere at 1100°C for 1 hour.
[0089] The honeycomb structure had a circular bottom with a diameter of 100 mm and a height (length of the cells in the flow path direction) of 100 mm. The cell density was 93 cells / cm. 2 The thickness of the partition walls was 101.6 μm, the porosity of the partition walls was 45%, and the average pore diameter of the partition walls was 8.6 μm. The thickness of the electrode layer was 0.3 mm, and the thickness of the base layer was 0.2 mm. When the electrical resistivity at 400°C was measured by the four-terminal method using test pieces made of the same material as the honeycomb structure, the electrode layer, and the base layer, the values were 5 Ωcm, 0.01 Ωcm, and 0.001 Ωcm, respectively.
[0090] (7. Fixing the electrodes) A comb-shaped electrode was placed on the honeycomb structure on which the base layer was formed, and the overlapping portions of each comb-shaped electrode and the base layer were laser-welded with a diameter of 0.5 mm in Examples 1 to 6 and Comparative Example 1. Ultrasonic welding was performed in Examples 7 to 11 and Comparative Example 2. Brazing was used for Examples 12 to 16 and Comparative Example 3. Next, for Examples 1 to 16, an antioxidant layer was formed in the following manner. The antioxidant layers in Examples 1 to 3 were provided as shown in Figure 4 (Embodiment 1), the antioxidant layers in Examples 7 to 9 were provided as shown in Figure 6 (Embodiment 1), and the antioxidant layers in Examples 12 to 14 were provided as shown in Figure 13(a). The antioxidant layers of Examples 4 and 10 were provided as shown in FIG. 7 (Embodiment 2), and the antioxidant layer of Example 15 was provided as shown in FIG. 13(b). The antioxidant layers of Examples 5 and 11 were provided as shown in FIG. 9 (Embodiment 3), and the antioxidant layer of Example 16 was provided as shown in FIG. 13(d). The antioxidant layer of Example 6 was provided as shown in FIG. 10 (Embodiment 4). SiO2-Al2O3-MgO was used as the material for the antioxidant layers in all of Examples 1 to 16. The thickness of each antioxidant layer is shown in Table 1 below.
[0091] (8. Oxidation Resistance Evaluation Test) An oxidation resistance evaluation test was conducted on a honeycomb structure with a pair of metal electrodes fixed using the above method. For the oxidation resistance evaluation test, a sample was placed in a heating furnace with a 5 mm diameter, 0.3 mm thick, disk-shaped base layer arranged in a 5 × 4 array with a center-to-center distance of 5 mm between adjacent base layers. The sample was then heated at 1000 °C for 50 hours in an air atmosphere. The resistance increase rate relative to the initial resistance value of the sample was used as an indicator of the oxidation state. A smaller resistance increase rate was determined to indicate a greater oxidation-inhibiting effect of the present invention. Resistance values were measured between two points on the base layer using a four-wire resistance measurement method using a Kelvin probe at a total of 12 points, and the average value was calculated. The conduction path of the sample was in the following order: (1) base layer surface, (2) base layer, (3) electrode layer, (4) base layer, and (5) base layer surface. The evaluation results are shown in Table 1.
[0092] [Table 1]
[0093] (9. Discussion) Regardless of the joining method, an oxidation suppression effect was obtained at the joining portion connecting the base layer and the metal electrode in all of Examples 1 to 16. Among these, the magnitude of the oxidation suppression effect differed depending on the form of the oxidation suppression layer, and further, the oxidation suppression effect differed among the forms of the oxidation suppression layer shown in Embodiment 1 (Examples 1 to 3, 7 to 9, and 12 to 14). Among the antioxidant layer configurations shown in Embodiment 1 (Examples 1 to 3, 7 to 9, and 12 to 14), Examples 3 and 14, in which the antioxidant layer was 200 μm thick, had the smallest antioxidant effect. This is thought to be because the thick antioxidant layer caused cracks in the antioxidant layer due to the difference in thermal expansion between the antioxidant layer and the base layer or metal electrode. For the same reason, when the cracking state was checked, Examples 1 and 12, in which the antioxidant layer was 10 μm thick, had smaller cracks than Examples 2 and 13, in which the antioxidant layer was 100 μm thick. Therefore, it is thought that the difference in antioxidant effect depending on the antioxidant layer thickness is due to cracks. Next, when comparing the forms of the antioxidant layer shown in Embodiments 2 and 4 in Examples 4 to 6, the oxidation inhibition effect was found to be as follows: form of antioxidant layer shown in Embodiment 3 of Example 5 < form of antioxidant layer shown in Embodiment 2 of Example 4 < form of antioxidant layer shown in Embodiment 4 of Example 6. This is thought to be because, as described above, an antioxidant layer is provided in Embodiment 2 of Example 4 as shown in FIG. 7, and an antioxidant layer is provided in Embodiment 3 of Example 5 as shown in FIG. 9, and therefore the amount of antioxidant film filled between the metal electrode and the underlayer affects the oxygen blocking ability. Furthermore, as described above, in embodiment 4 of example 6, an anti-oxidation layer is provided as shown in FIG. 10, and the entire periphery of the joining portion is covered with the anti-oxidation layer. Therefore, even if oxygen penetrates through a part of the anti-oxidation layer due to a crack or the like, the anti-oxidation effect can be maintained, and it is considered that this has the greatest anti-oxidation effect. [Explanation of symbols]
[0094] 10 Electrically heated carrier 11 Pillar honeycomb structure 12 Peripheral wall 13a, 13b electrode layer 14a, 14b metal electrode 15 Electrode section 16 Base layer 17 Second Underlayer or Electrode Layer 18 cells 19 Bulkhead 20, 20a, 20b, 20c, 20d joint site 21, 21a, 21b, 21c, 21d, 21e, 21f, 21g, 21h, 21i Antioxidant layer 22 Gap 23 Coat layer 24 Fixed layer
Claims
1. A ceramic pillar-shaped honeycomb structure having an outer peripheral wall and partition walls disposed inside the outer peripheral wall and defining a plurality of cells that form flow paths penetrating from one end face to the other end face; An electrode layer disposed on a surface of an outer peripheral wall of the columnar honeycomb structure; a conductive underlayer provided on the electrode layer; a metal electrode connected to the underlayer by a bonding portion; an anti-oxidation layer for protecting the joint from exhaust gas; Equipped with An electrically heated carrier, in which the antioxidant layer is provided from at least midway along the side of the base layer over a portion of the outer surface of the metal electrode in a direction from the outer surface of the electrode layer to the outer surface of the metal electrode so as to seal the gap between the base layer and the metal electrode.
2. A ceramic pillar-shaped honeycomb structure having an outer peripheral wall and partition walls disposed inside the outer peripheral wall and defining a plurality of cells that form flow paths penetrating from one end face to the other end face; An electrode layer disposed on a surface of an outer peripheral wall of the columnar honeycomb structure; a conductive underlayer provided on the electrode layer; a metal electrode connected to the underlayer by a bonding portion; an anti-oxidation layer for protecting the joint from exhaust gas; Equipped with An electrically heated carrier, wherein the anti-oxidation layer is provided between the base layer and the metal electrode and spaced apart from the joint portion.
3. An electrically heated carrier as described in claim 1 or 2, wherein the electrode layer arranged on the surface of the outer wall of the columnar honeycomb structure is a pair of electrode layers arranged on the surface of the outer wall of the columnar honeycomb structure so as to face each other across the central axis of the columnar honeycomb structure.
4. An electrically heated carrier according to any one of claims 1 to 3; A metallic tubular member for holding the electrically heated carrier; An exhaust gas purification device having the above structure.
Citation Information
Patent Citations
Ceramic heater and its manufacturing method
JP2003347012A
Exhaust gas treatment device
JP2016014395A
Honeycomb structure and manufacturing method therefor
JP2016074589A
Conductive honeycomb structure
JP2018172258A
Electric heating-type catalyst carrier
JP2019171345A