A process for producing a composite structure with a thin layer of monocrystalline SiC on a carrier substrate made of SiC
The described process addresses the challenges of creating high-quality composite structures with single crystal SiC on polycrystalline substrates by using epitaxial growth, ion implantation, and low-temperature deposition to achieve efficient vertical electrical conduction and thermal management, thus enhancing the performance and reducing costs.
Patent Information
- Application Number
- JP2022523651
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-03-27
- Filing Date
- 2020-10-26
- Publication Date
- 2024-12-04
- Estimated Expiration
- 2040-10-26
AI Technical Summary
Existing methods for creating composite structures with a thin layer of single crystal SiC on a carrier substrate face challenges such as high cost, complexity, and the formation of amorphous layers that affect vertical electrical conduction, especially when using polycrystalline SiC substrates, due to difficulties in achieving high-quality direct bonding and controlling surface conditions.
A process involving epitaxial growth of a single crystal SiC donor layer, ion implantation to create a buried brittle plane, followed by direct liquid injection-chemical vapor deposition at low temperatures to form a carrier layer, separation along the brittle plane, and heat treatment to crystallize the carrier layer, ensuring high-quality electrical conductivity and thermal properties.
The process results in a high-quality composite structure with low extended defects, enabling efficient vertical electrical conduction and thermal management, suitable for power devices, while reducing production costs and complexity.
Smart Images

Figure 0007594585000001 
Figure 0007594585000002 
Figure 0007594585000003
Abstract
Description
[Technical field]
[0001] The present invention relates to the field of semiconductor materials for microelectronic components, and more particularly to a process for producing a composite structure comprising a thin layer of monocrystalline silicon carbide on a carrier substrate made of silicon carbide. [Background technology]
[0002] Interest in silicon carbide (SiC) has increased significantly over the last few years because of this semiconductor material's ability to increase its ability to process energy. SiC is being used more and more extensively to create innovative power devices, particularly to meet the needs of emerging areas of electronics such as electric vehicles.
[0003] Power devices and integrated power supply systems based on monocrystalline silicon carbide are able to manage much higher power densities and to do so with smaller active area dimensions than their traditional silicon analogues. To further limit the dimensions of power devices on SiC, it is advantageous to create vertical components instead of lateral ones. For this purpose, the SiC structure must allow vertical electrical conduction between electrodes placed on the front and rear sides of the structure.
[0004] However, monocrystalline SiC substrates intended for the microelectronics industry remain expensive and difficult to supply in large sizes. It is therefore advantageous to utilize thin layer transfer solutions to create composite structures that typically comprise a thin layer of monocrystalline SiC on an inexpensive carrier substrate. One well-known thin layer transfer solution is the Smart Cut™ process, which is based on implanting light ions and texturing by direct bonding. Such a process makes it possible to create composite structures that comprise, for example, a thin layer of c-SiC taken from a monocrystalline SiC (c-SiC) donor substrate in direct contact with a polycrystalline SiC (p-SiC) carrier substrate, allowing vertical electrical conduction. However, it remains difficult to achieve high-quality direct bonding by molecular adhesion between two substrates made of c-SiC and p-SiC, because of the complexity of controlling the surface condition and roughness of these substrates.
[0005] Various methods derived from this process are also known from the prior art. For example, F. Mu et al. (ECS Transactions, 86(5)3-21, 2018) perform direct bonding after activating the surface to be textured by irradiation with argon ("surface activated bonding" or SAB): such a treatment prior to bonding produces a very high density of side bonds, which promote the formation of covalent bonds at the textured interface and therefore high bonding energy. However, this method has the drawback of producing an amorphous layer at the surface of the monocrystalline SiC donor substrate, which has a negative effect on the vertical electrical conduction between the thin layer of c-SiC and the carrier substrate made of p-SiC.
[0006] A solution to solve this problem is proposed, more particularly, in document EP 3168862, which involves the implantation of dopant species into the amorphous layer in order to restore its electrical properties. The main drawback of this approach is its complexity and therefore its cost.
[0007] Also known is US Pat. No. 8,436,363, which describes a process for producing a composite structure comprising a thin layer of c-SiC disposed on a metal carrier substrate, the thermal expansion coefficient of which matches the thermal expansion coefficient of the thin layer.
[0008] This creation process is forming a buried brittle plane in a c-SiC donor substrate, the buried brittle plane defining a thin layer between the buried brittle plane and a front surface of the donor substrate; depositing a layer of metal, e.g., tungsten or molybdenum, on a front surface of the donor substrate to form a carrier substrate having a thickness sufficient to act as a stiffener; Separating along the embedded brittle plane to form a composite structure comprising, on the one hand, the metal carrier substrate and the thin layer of c-SiC, and, on the other hand, a remnant of the c-SiC donor substrate. Includes.
[0009] However, such a fabrication process is incompatible when the material forming the carrier substrate is p-SiC, requiring deposition at temperatures above 1200° C. (the usual temperature for the fabrication of p-SiC). More specifically, at these high temperatures, the growth rate of the cavities present in the buried brittle plane is faster than that of the p-SiC layer, and the thickness required for the stiffening effect is not reached before blistering begins to occur, which is associated with deformation of the layer aligned perpendicular to the cavities.
[0010] Regardless of the layer transfer technique used, the further problem arises of providing a composite structure comprising a thin c-SiC layer of very high quality, and more particularly, free of extended defects (or having a very low density of extended defects), which tend to adversely affect the performance and reliability of power devices intended to be fabricated on said thin layer. Summary of the Invention [Problem to be solved by the invention]
[0011] The present invention relates to an alternative solution to the prior art solutions and aims to overcome in whole or in part the above-mentioned drawbacks, and more particularly to a process for producing a composite structure comprising a high-quality thin layer of SiC on a carrier substrate made of SiC. [Means for solving the problem]
[0012] The present invention relates to a process for making a composite structure comprising a thin layer of single crystal silicon carbide disposed on a carrier substrate made of silicon carbide.
[0013] The process is a) providing an initial substrate made of single crystal silicon carbide; b) epitaxially growing a single crystal silicon carbide donor layer on the initial substrate to form a donor substrate, the donor layer having a crystal defect density lower than the crystal defect density of the initial substrate; c) ion implanting a light species into the donor layer to form a buried brittle plane, said buried brittle plane defining a thin layer boundary between said buried brittle plane and a free surface of the donor layer; d) forming a carrier layer directly on the free surface of the donor layer by direct liquid infusion-chemical vapor deposition at a temperature below 1000° C., said carrier layer being formed by an at least partially amorphous SiC matrix; e) Separation along the embedded brittle plane to form, on the one hand, an intermediate composite structure comprising a thin layer on a carrier layer and, on the other hand, a remnant of the donor substrate; f) performing a heat treatment at a temperature between 1000° C. and 1800° C. applied to the intermediate composite structure to crystallize the carrier layer and form a polycrystalline carrier substrate; g) a step of mechanical and / or chemical treatment of the composite structure, said treatment being applied to the free face of the carrier substrate, to the rear face of the composite structure, and / or to the free face of the thin layer (10), to the front face of the composite structure. Includes.
[0014] According to other advantageous and non-limiting characteristics of the present invention, taken alone or in any technically feasible combination, The deposition step d) is carried out at a temperature between 100° C. and 700° C., or more preferably between 200° C. and 600° C.; The deposition step d) is carried out at a pressure between 1 and 500 Torr; The precursors used during the deposition step d) are selected from polysilylethylene and disilabutane; At the end of the deposition step d), the carrier layer has a thickness of 10 microns or more, or even 50 microns or more, or even 100 microns or more, or even 200 microns or more; Chemical etching, mechanical grinding and / or chemical-mechanical polishing is applied to the free side of the carrier layer between steps d) and e); Step a) includes forming a single crystal conversion layer on an initial substrate to convert basal plane dislocation defects of the initial substrate into threading edge dislocation defects; The epitaxial growth step b) is carried out at a temperature higher than 1200° C., preferably between 1500° C. and 1650° C.; The separation step e) is carried out at a temperature higher than the deposition temperature of step d); The separation step e) takes place during the deposition step d), preferably at the end of step d); The separation step e) and the crystallization step f) occur during the same heat treatment; Step g) comprises simultaneous mechanical and chemical polishing of the front and rear surfaces of the composite structure; Reconditioning the donor substrate remnant for reuse as an initial substrate or as a donor substrate.
[0015] Other features and advantages of the present invention will become apparent from the following detailed description of the invention, which proceeds with reference to the accompanying drawings. [Brief description of the drawings]
[0016] [Figure 1] FIG. 2 illustrates a composite structure produced by a production process according to the present invention. [Figure 2a] FIG. 2 illustrates steps of the creation process according to the present invention. [Figure 2b] FIG. 2 illustrates steps of the creation process according to the present invention. [Figure 2c] FIG. 2 illustrates steps of the creation process according to the present invention. [Figure 2d] FIG. 2 illustrates steps of the creation process according to the present invention. [Figure 2e] FIG. 2 illustrates steps of the creation process according to the present invention. [Figure 2f] FIG. 2 illustrates steps of the creation process according to the present invention. [Figure 2g] FIG. 2 illustrates steps of the creation process according to the present invention. [Figure 3a] FIG. 2 illustrates steps of the creation process according to the present invention. [Figure 3b] FIG. 2 illustrates steps of the creation process according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] In this description, the same reference numbers of the figures may be used for the same type of elements. The figures are schematic representations that are not to scale for ease of reading. More specifically, the thickness of the layers along the z-axis is not to scale with respect to the lateral dimensions along the x- and y-axes, and the relative thicknesses of the layers with respect to one another are not necessarily respected in the figures.
[0018] The present invention relates to a process for producing a composite structure 1 comprising a thin layer 10 of monocrystalline silicon carbide arranged on a carrier substrate 20 made of silicon carbide (FIG. 1). The carrier substrate 20 is advantageously polycrystalline ("p-SiC" is used to designate polycrystalline SiC).
[0019] The process first comprises step a) of providing an initial substrate 11 made of monocrystalline silicon carbide (FIG. 2a). Throughout the remainder of the description, "c-SiC" will be used to refer to monocrystalline silicon carbide.
[0020] The initial substrate 11 is preferably in the form of a wafer having a diameter of 100 mm, 150 mm, or 200 mm, or even 300 mm, or even 450 mm, and a thickness typically between 300 and 800 microns. The initial substrate 11 has a front surface 11a and a rear surface 11b. The surface roughness of the front surface 11a is advantageously chosen to be smaller than 1 nm Ra (average roughness), measured by atomic force microscopy (AFM) on a 20 micron x 20 micron scan.
[0021] The process then comprises a step b) of epitaxially growing a monocrystalline silicon carbide donor layer 110 on the initial substrate 11 to form a donor substrate 111 (FIG. 2b). The epitaxial growth step is performed such that the donor layer 110 has a lower crystal defect density than the crystal defect density of the initial substrate 11.
[0022] Typically, the initial substrate 11 made of c-SiC is of the 4H or 6H polytype, has an offcut angle of less than 4.0° relative to the <11-20> crystal axis ±0.5°, and has a lattice constant of 5 / cm. 2 Less than or equal to 1 / cm 2 For example, when N (nitrogen) doped, the initial substrate 11 preferably has a resistivity between 0.015 ohm.cm and 0.030 ohm.cm. Typically 3000 / cm 2 An initial substrate 11 may be selected that has a low density of basal plane dislocation (BPD) defects of less than 1500 / cm 2 Substrates of c-SiC with BPD densities on the order of 1000 nm are reasonably available, making their supply easy.
[0023] At the end of the process of the invention, it is desirable that the donor layer 110 from which the thin c-SiC layer 10 of the composite structure 1 will be formed has a higher crystalline quality than the initial substrate 11 in order to meet the specifications required for the vertical components to be made on said thin layer 10. The reason is that various types of extended defects are present in the c-SiC layer or substrate. These extended defects may affect the performance and reliability of the components. More specifically, BPD type defects are fatal for bipolar components: Shockley stacking faults (or SSFs) extend from dislocations when energy is available for the recombination of electron-hole pairs. The extension of SSF stacking faults inside the active area of the component leads to an increase in the conductive state resistance of the component.
[0024] Therefore, the c-SiC donor layer 110 has a thickness of 1 / cm 2 The BPD defect density is
[0025] For this reason, the epitaxial growth step b) is carried out at a temperature higher than 1200° C., preferably between 1500° C. and 1650° C. The precursors used are silane (SiH4), propane (C3H8) or ethylene (C2H4); the carrier gas may be hydrogen with or without argon.
[0026] The low concentration of BPD defects in the donor layer 110 is obtained by favoring the conversion of BPD defects present in the initial substrate 11 into threading edge dislocations (TEDs).
[0027] According to a particular embodiment, step a) comprises the formation of a monocrystalline conversion layer 13, preferably based on c-SiC, in order to maximize the conversion of BPD defects in the initial substrate 11 into TED defects (FIG. 3a). For this, it is advantageous to choose a low cutting angle of approximately 4° for the initial c-SiC substrate 11, to increase the in situ etching carried out before the epitaxial growth, to target a high growth rate (typically higher than 5 μm / h) and finally to choose growth conditions for the monocrystalline conversion layer 13 with a C / Si ratio in the precursor flows of approximately 1.
[0028] Step b) then consists in carrying out epitaxial growth of a donor layer 110 on said conversion layer 13 (FIG. 3b). According to this particular embodiment, the 1 / cm 2 Less than or equal to 0.1 / cm 2 It is also possible to obtain a donor layer 110 of c-SiC with a smaller BPD defect density. Moreover, at the end of the process according to the invention, the probability of bipolar degradation (probability of holes arriving below the BPD / TED conversion point) is negligible (<0.1%) and the monocrystalline conversion layer 13 is not intended to be transferred into the composite structure 1. Prior art aimed at reducing bipolar degradation involves the use of a (1 E 18at / cm 3 The aim of the present invention is to incorporate a recombination layer (doped with nitrogen in excess of 10 μm) having a thickness of 10 μm and a thickness of 5 μm. E 18 / cm 3At the expense of a higher concentration, the probability of holes being present can be reduced to 0.1% relative to the basis structure without this recombination layer. In the present invention, since the single crystal conversion layer 13 is not transferred, the probability of holes reaching the nucleation point of bipolar degradation (BPD-TED conversion point or any BPD point) is at least less than 0.1%, or even very close to 0%.
[0029] It is noted that a conventional sequence of cleaning or etching of the initial substrate 11 aimed at removing particulate matter, metallic or organic contaminants or part or all of the native oxide layer possibly present on its front surface 11a may be carried out prior to the epitaxial growth step b).
[0030] The fabrication process according to the invention also comprises a step c) of ion implantation of light species into the donor layer 110 up to a given depth indicating the desired thickness of the thin layer 10, and in any case not reaching the initial substrate 11 (and / or the conversion layer 13, if present). This implantation produces a buried brittle plane 12 in the donor layer 110, which defines the boundary of the thin layer 10 between said buried brittle plane 12 and the free surface 11a of the donor layer 110 (Figure 2c).
[0031] The light species implanted are preferably hydrogen, helium or a combination of these two species co-implanted. As is well known for the Smart-Cut™ process, these light species will form microcavities around a given depth distributed in a thin layer parallel to the free surface 11a of the donor layer 110, i.e. parallel to the plane (x,y) of the drawing. This thin layer is called, for simplicity, the buried brittle plane 12.
[0032] The energy for implanting the light species is selected to reach a given depth within donor layer 110 .
[0033] Typically, the hydrogen ions are irradiated at energies between 10 keV and 250 keV and at 50 keV to define a thin layer 10 having a thickness of about 100 nm to 1500 nm. E 16 / cm 2 and 1 E 17 / cm 2 The implantation will be carried out at a dose between 0.01 and 0.1.
[0034] It should be noted that a protective layer can be deposited on the free surface of the donor layer 110 prior to the ion implantation step. This protective layer can be made of a material such as silicon oxide or silicon nitride, for example.
[0035] The process according to the invention then comprises a step of direct liquid infusion-chemical vapor deposition at a temperature below 1000° C., and preferably below 900° C., to form a carrier layer 20′ directly above the free surface of the donor layer 110 (FIG. 2d). The deposition step d) may be carried out at a temperature between 100° C. and 800° C., between 100° C. and 700° C., or even more advantageously between 200° C. and 600° C. The pressure in the deposition chamber is preferably defined to be between 1 and 500 Torr.
[0036] The DLI-CVD deposition technique offers high yields between delivered materials (precursors) and achieved deposition thicknesses without the need to use chlorine-containing precursors, limiting cost and environmental constraints.
[0037] Preferably, the DLI-CVD deposition includes a disilabutane precursor or a polysilylethylene precursor, said precursor being pure or diluted. Other precursors such as methyltrichlorosilane, ethylenetrichlorosilane, dichloromethylvinylsilane, tetraethylsilane, tetramethylsilane, diethylmethylsilane, bistrimethylsilylmethane, or hexamethyldisilane may optionally be used.
[0038] Such a technique is described in a paper by Guilhaume Boisselier (2013, "Depot chimique en phase vapeur de carbures de chrome, de silicium et d'hafnium assiste par injection liquide pulsee [Pulsed liquid injection-chemical vapor deposition of chromium, silicon and hafnium carbide]") for the application of deposition of ceramic coatings onto parts, thereby protecting them, for example, during processing at very high temperatures of steel or alloy parts.
[0039] The applicant has developed a DLI-CVD deposition step d) for the formation of a carrier layer 20' on a c-SiC donor layer 110 in order to obtain, at the end of the fabrication process, a composite structure 1 intended for a completely different application, namely the microelectronics sector.
[0040] The deposited carrier layer 20' forms a SiC matrix that includes amorphous SiC and reaction products that originate from the precursors used during deposition and are formed from carbon chains, and may optionally include crystalline SiC particles.
[0041] The DLI-CVD technique can provide deposition rates of 10 microns / hour or more, or even faster than 50 microns / hour, or even faster than 100 microns / hour. Taking into account the average deposition temperature, the deposition rate does not have to be fast (other than for obvious economic reasons), since the thermally activated growth of the cavities of the buried brittle plane 12 remains slow within these temperature ranges, making it easy to achieve a thickness of the carrier layer 20' that is able to ensure a stiffening effect on the buried brittle plane 12.
[0042] At the end of step d), the carrier layer 20' has a thickness of 10 microns, 50 microns, 100 microns or more, or even 200 microns or more. The laminate 211 obtained by step d) comprises a carrier substrate 20' arranged on a donor layer 110, which is itself arranged on an initial substrate 11.
[0043] The process according to the invention then comprises a step e) of separation along the embedded brittle plane 12 to form, on the one hand, an intermediate composite structure 1' and, on the other hand, a remnant 111' of the donor substrate (FIG. 2e).
[0044] According to an advantageous embodiment, the separation step e) is carried out by applying a heat treatment to the stack 211 at a separation temperature higher than the temperature of the deposition of step d). More precisely, the microcavities present in the buried brittle plane 12 follow a growth rate until a breaking wave is initiated, which propagates over the entire extent of the buried brittle plane 12 and results in a separation between the intermediate composite structure 1' and the remainder 111' of the initial substrate. In practice, that temperature may be between 950 and 1200°C, and preferably between 1000 and 1200°C, depending on the implantation conditions of step c).
[0045] According to an alternative embodiment, the separation step e) is performed by applying a mechanical stress to the laminate 211, optionally preceded by a heat treatment embrittling the embedded brittle plane 12. The stress may for example be performed by inserting a tool (for example: a razor blade) against the embedded brittle plane 12. By way of example, the separation stress may be of the order of a few GPa, preferably greater than 2 GPa.
[0046] According to yet another embodiment, the separation step e) along the buried brittle plane 12 is performed during the DLI-CVD deposition step d) or as soon as the DLI-CVD deposition step d) is finished, more particularly when the deposition temperature is in the range of 900°C to 1000°C.
[0047] The manufacturing process according to the invention then comprises step f) of carrying out a heat treatment at a temperature between 1000° C. and 1800° C. applied to the intermediate composite structure 1 ′ to crystallize the carrier layer 20 ′ and form a polycrystalline carrier substrate 20 .
[0048] The annealing atmosphere may include gases such as argon, nitrogen, hydrogen, helium, or mixtures of these gases, among others.
[0049] Such annealing has the effect of removing hydrogen from the carrier layer 20' and resulting in crystallization of the SiC matrix in the form of polycrystalline SiC.
[0050] Conventional furnaces for processing multiple structures simultaneously (batch annealing) may be used to carry out the crystallization heat treatment, the typical duration of which is between a few minutes and a few hours.
[0051] It may optionally be envisaged to carry out a crystallization heat treatment in situ within the DLI deposition chamber, for a typical duration on the order of a few minutes.
[0052] Advantageously, the temperature rise and fall ramps will be limited to, for example, less than 20° / min, less than 5° / min, or even less than 1° / min, to limit the appearance of cracks or structural defects in the crystalline layer.
[0053] After step f), a composite structure 1 is obtained comprising a thin layer 10 of monocrystalline silicon carbide arranged on a carrier substrate 20 made of polycrystalline silicon carbide.
[0054] The deposition parameters (step d) and the crystallization annealing parameters (step f) are set so that the carrier substrate 20 is Good electrical conductivity, i.e., less than 0.03 ohm.cm, or even less than 0.01 ohm.cm; High thermal conductivity, i.e., 150W.m -1 .K -1 or more than 200W.m -1 .K-1 That's all, and a thermal expansion coefficient close to that of the thin layer 10, i.e., 3.8 at room temperature. E -6 / K and 4.2 E Between -6 / K It is determined that the
[0055] To obtain these properties, the following structural features are preferably targeted for the carrier substrate 20: polycrystalline structure, 3C SiC type grains,
[0111] orientation, average size between 1 μm and 50 μm in the major plane of the substrate, N-type doping for a final resistivity of 0.03 ohm.cm or even 0.01 ohm.cm or less.
[0056] Additionally, a non-insulating interface between the donor layer 110 and the carrier substrate 20 is preferably targeted. Typically, 1 mohm.cm 2 A smaller interface resistivity is typically expected. To ensure interface electrical conductivity, removal of the native oxide present on the free surface of the donor layer 110 is performed by HF deoxidation by wet or dry route prior to deposition step d). Alternatively, overdosing of at least the first few deposited nanometers of the carrier layer 20' may be performed by introducing dopant species during DLI-CVD deposition step d). It should be noted that in general, dopant species may be introduced (in different doses) during deposition step d) depending on the level of doping and the electrical conductivity targeted for the carrier substrate 20, which conductivity will be effective at the end of the crystallization annealing of step f).
[0057] Also advantageously, prior to deoxidation and / or formation of the carrier layer 20', a cleaning sequence is applied to the donor substrate 111 to remove all or part of any particulate matter, metal or organic contaminants possibly present on the front surface of the substrate 111.
[0058] As is known per se, at the end of the separation step e), the free surface 10a of the thin layer 10 of the composite structure 1 has a surface roughness of between 5 nm RMS and 100 nm RMS (measured using an atomic force microscope (AFM) on a scan of 20 microns x 20 microns).
[0059] Therefore, a step g) of mechanical and / or chemical treatment of the composite structure 1 is envisaged in order to smooth the free surface 10a of the thin layer 10 and to correct the thickness uniformity of the composite structure 1 (FIG. 2f).
[0060] Step g) may comprise a mechanical chemical polishing (MCP) of the free surface 10a of the thin layer 10, typically involving the removal of material of the order of 50 nm to 1000 nm, to obtain a final roughness smaller than 0.5 nm RMS (on an AFM field of view of 20 μm×20 μm), or even smaller than 0.3 nm. Step g) may comprise a chemical or plasma treatment (cleaning or etching), for example a SC (Standard Clean) 1 / SC2 (Standard Clean 1 / Standard Clean 2) type cleaning and / or HF (Hydrofluoric Acid) cleaning and / or N2, Ar, CF4 plasma, etc., to further improve the quality of the free surface 10a of the thin layer 10.
[0061] It is important to note that crystallization of the carrier layer 20' often causes cracks or structural defects in the crystalline layer (forming the carrier substrate 20), which affect the mechanical and electrical qualities of the crystalline layer.
[0062] Therefore, step g) is carried out to improve the thickness uniformity of the carrier substrate 20 and also the roughness of its rear surface 20b, to remove cracks and structural defects. This may include mechanical chemical polishing (MCP) and / or chemical (etching or cleaning) and / or mechanical (grinding) treatment of the rear surface 20b of the carrier substrate 20. The thickness removed on the rear surface may be between about 100 microns and a few microns.
[0063] A roughness of less than 0.5 nm RMS (measured using an atomic force microscope (AFM) over a 20 micron x 20 micron field of view) is desired for creating vertical components for which at least one metal electrode will be present on the rear surface 20b of the composite substrate 1.
[0064] Polishing or grinding of the edges of the composite structure 1 may be carried out during this step g) in order to adapt its circular contour shape and cutting edge waste to the requirements of the microelectronic fabrication process.
[0065] It should be noted that a contamination-resistant or restrictive treatment applied to the rear surface 20b of the carrier substrate 20 may optionally be applied to the free surface of the carrier layer 20' immediately prior to the separation step e), i.e. before the front surface 10a of the composite structure 1 is exposed, in order to limit its contamination during processes such as, in particular, chemical etching or mechanical polishing (grinding).
[0066] According to an advantageous embodiment, the mechanical-chemical treatment step g) comprises simultaneous polishing (MCP) of the front 10a and rear 20b faces of the composite structure 1 in order to smooth said structure and improve its thickness uniformity. The polishing parameters may be different between the front and rear faces, the smoothing of c-SiC surfaces and the smoothing of p-SiC surfaces usually requiring different consumables. The mechanical component of polishing is more particularly advantageous for the rear face 20b when the carrier substrate 20 is made of p-SiC, in order to limit peripheral attack of the grain joints by the chemical component of polishing. By way of example, the rotation speed (polishing head and plate), pressure, concentration and physical properties of the polishing agent (i.e. diamond nanoparticle diameter between about 10 nm and 1 μm) may be modified to accentuate the mechanical component.
[0067] Optionally, a step g') of heat treatment at a temperature between 1000° C. and 1800° C. for about one hour and up to several hours is carried out after step g). The purpose of this step is to stabilize the composite structure 1 by securing structural or surface defects still present in and / or on the thin layer 10 and, if necessary, by substantially evolving the crystal structure of the carrier substrate 20 so that the structure 1 is suitable for a subsequent heat treatment at high temperature required for the creation of a part on the thin layer 10.
[0068] The process according to the invention may also comprise a second step h) of epitaxial growth of a further layer 10' of monocrystalline silicon carbide on the thin layer 10 of the composite structure 1 (FIG. 2g). Such a step is applied when a working layer 100 of a significant thickness is required, typically for the creation of components of the order of 5 microns to 50 microns.
[0069] For the composite structure 1, it may be chosen to limit the temperature applied during this step h) in order to limit the stresses induced in the working layer 100 (corresponding to the combination of the thin layer 10 and the further layer 10').
[0070] Finally, the preparation process may include a step of reconditioning the donor substrate remainder 111' in order to reuse it as initial substrate 1 or as donor substrate 111. Such a reconditioning step is based on one or more treatments of face 110'a by mechanical-chemical polishing and / or by mechanical grinding and / or by wet or dry chemical etching of the surface or edges (Figure 2e).
[0071] Preferably, the thickness of the donor layer 110 formed in step b) is defined such that the remainder 111' of the donor substrate 111 can be reused as the donor substrate 111 at least twice.
[0072] Preferably, when the conversion layer 13 is present, care will be taken to keep said layer intact, i.e. always to maintain a portion of the donor layer 10 on the remainder 111' of the donor substrate. Thus, when the portion of the donor layer 10 is insufficient to create the composite structure 1, only the step of epitaxial growth of the donor layer 10 is necessary, and no prior step of growth of the conversion layer 13 is necessary. EXAMPLES
[0073] According to a non-limiting exemplary embodiment, the initial substrate 11 provided in step a) of the fabrication process is a wafer made of c-SiC of the 4H polytype, with an orientation of 4.0° relative to the <11-20> axis ±0.5°, a diameter of 150 mm and a thickness of 350 μm.
[0074] A conventional RCA cleaning sequence (Standard Clean 1 + Standard Clean 2) followed by Caro's acid (a mixture of sulfuric acid and hydrogen peroxide) and then HF (hydrofluoric acid) is performed on the initial substrate 11 prior to step b) of epitaxial growth of the c-SiC donor layer 110.
[0075] The growth is carried out in an epitaxy chamber using precursors such as silane (SiH4) and propane (C3H8) or ethylene (C2H4) at a temperature of 1650° C., producing a c-SiC donor layer 110 with a thickness of 30 microns (growth rate: 10 microns / hour). The donor layer has a thickness of 1 / cm 2 The BPD defect density is on the order of .
[0076] Hydrogen ions penetrate the free surface of the donor layer 110 with an energy of 150 keV and E 16H+ / cm 2 A buried brittle plane 12 is thus created in the initial substrate 11 to a depth of about 800 nm.
[0077] A RCA+Caro's acid cleaning sequence is performed on the donor substrate 111 to remove possible contaminants from the free surface of the donor layer 110.
[0078] DLI-CVD deposition is carried out on the donor layer 110 at a temperature of 800° C. with disilabutane (DSB) at a pressure of 50 Torr for 60 minutes in order to reach a thickness of at least 150 microns on the carrier substrate 20. Under these conditions, the carrier layer 20′ is deposited in the form of an amorphous SiC matrix containing reaction products originating from the deposition precursors.
[0079] An annealing at 1000° C. is then applied to the laminate 211 for 50 minutes, during which detachment is carried out on the embedded brittle plane 12. At the end of this detachment step e), the intermediate composite structure 1′ formed by the thin layer 10 and the carrier layer 20′ is separated from the remainder 111′ of the donor substrate.
[0080] A crystallization heat treatment at 1200° C. for 1 hour under argon atmosphere is then applied to said intermediate composite structure 1 ′ to form the poly-SiC carrier substrate 20 of the composite structure 1 .
[0081] Alternatively, separation and crystallization may be carried out during the same heat treatment, for example at 1200° C. under a neutral atmosphere.
[0082] Mechanical grinding of the rear face of the carrier substrate 20, removing approximately 15 to 30 microns, makes it possible to eliminate cracks and structural defects generated by the crystallization of the SiC matrix.
[0083] One or more mechanical-chemical polishing operations are then performed to restore the surface roughness of the back surface of the thin layer 10 and carrier substrate 20, followed by a conventional cleaning sequence.
[0084] Of course, the invention is not limited to the described embodiments and examples, and variations in its implementation may be envisaged without departing from the scope of the invention as defined by the claims.
Claims
1. A process for producing a composite structure (1) comprising a thin layer (10) of monocrystalline silicon carbide disposed on a carrier substrate (20) made of silicon carbide, comprising: a) providing an initial substrate (11) made of monocrystalline silicon carbide; b) epitaxially growing a donor layer (110) of monocrystalline silicon carbide on the initial substrate (11) to form a donor substrate (111), the donor layer (110) having a crystal defect density lower than the crystal defect density of the initial substrate (11); c) ion implantation of light species into the donor layer (110) to form a buried brittle plane (12), the buried brittle plane (12) defining the boundary of the thin layer (10) between the buried brittle plane (12) and a free surface of the donor layer (110); d) forming a carrier layer (20') directly on the free surface of the donor layer (110) by direct liquid infusion-chemical vapor deposition at a temperature below 1000°C, the carrier layer (20') being formed at least in part by an amorphous SiC matrix; e) separation along said embedded brittle plane (12) to form, on the one hand, an intermediate composite structure (1′) comprising said thin layer (10) on said carrier layer (20′) and, on the other hand, a remainder (111′) of the donor substrate; f) a heat treatment at a temperature between 1000°C and 1800°C applied to the intermediate composite structure (1') to crystallize the carrier layer (20') and form the polycrystalline carrier substrate (20); g) a step of mechanical and / or chemical treatment of the composite structure (1), the mechanical and / or chemical treatment being applied to the free face of the carrier substrate (20) as the rear face of the composite structure (1) and / or to the free face of the thin layer (10) as the front face of the composite structure (1); The process of creating, including
2. 2. The process of claim 1, wherein step d) is carried out at a temperature between 100°C and 700°C.
3. 3. The process of claim 1 or 2, wherein step d) is carried out at a pressure between 1 Torr and 500 Torr.
4. The process of any one of claims 1 to 3, wherein the precursors used during step d) are selected from polysilylethylene and disilabutane.
5. The producing process according to any one of claims 1 to 4, wherein at the end of step d), the carrier layer (20') has a thickness of 10 microns or more.
6. The producing process according to any one of claims 1 to 5, wherein chemical etching, mechanical grinding and / or chemical-mechanical polishing is applied to the free side of the carrier layer (20') between steps d) and e).
7. 7. The producing process according to any one of claims 1 to 6, wherein step a) comprises the formation of a single crystal conversion layer (13) on the initial substrate (11) in order to convert basal plane dislocation defects of the initial substrate (11) into threading edge dislocation defects.
8. The process of any one of claims 1 to 7, wherein step b) is carried out at a temperature above 1200°C.
9. The process of making according to any one of claims 1 to 8, wherein said step e) is carried out at a temperature higher than the deposition temperature of step d).
10. The making process according to any one of claims 1 to 8, wherein said step e) occurs during said step d).
11. The making process according to any one of claims 1 to 9, wherein said steps e) and f) are carried out during the same heat treatment.
12. The process of making according to any one of the preceding claims, wherein step g) comprises simultaneous mechanical and chemical polishing of the front and rear faces of the composite structure (1).
13. The process of making according to any one of claims 1 to 12, comprising a step of reconditioning the remnant (111') of the donor substrate for reuse as an initial substrate or as a donor substrate.
Citation Information
Patent Citations
Semiconductor device
JP1989220458A
Film deposition apparatus, film deposition method and method for feeding process gas
JP2005307233A
Method for manufacturing single crystal gallium nitride substrate
JP2007230810A
Manufacturing method of multilayer-structured silicon carbide substrate
JP2007273524A
PRODUCTION OF SiC COMPOSITE SUBSTRATE
JP2017057102A