Non-oriented electrical steel sheet and its manufacturing method
The non-oriented electrical steel sheet with optimized Si, Mn, Al, P, and As composition, combined with controlled manufacturing processes, addresses the challenge of achieving low iron loss and high magnetic flux density, enhancing productivity and cost-effectiveness.
Patent Information
- Application Number
- JP2022537536
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-12-19
- Filing Date
- 2020-12-09
- Publication Date
- 2024-12-04
- Estimated Expiration
- 2040-12-09
AI Technical Summary
Existing non-oriented electrical steel sheets face challenges in achieving low iron loss and high magnetic flux density while maintaining productivity and cost-effectiveness, as conventional methods often result in increased manufacturing costs and deteriorated magnetic properties due to improper control of alloying elements and manufacturing processes.
A non-oriented electrical steel sheet composition with specific ratios of Si, Mn, Al, P, and As, along with controlled manufacturing processes including hot-rolling, cold-rolling, and final annealing, to optimize texture and magnetic properties, ensuring a uniform grain size distribution and reduced residual stress.
The solution achieves a non-oriented electrical steel sheet with improved magnetism, low iron loss, and high magnetic flux density, maintaining productivity and reducing manufacturing costs by optimizing the addition of alloying elements and process controls.
Smart Images

Figure 0007594590000001 
Figure 0007594590000002 
Figure 0007594590000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a non-oriented electrical steel sheet and a manufacturing method thereof, and more particularly to a non-oriented electrical steel sheet having improved magnetic properties by appropriately adding As and P to improve the texture and the manufacturing method thereof. [Background technology]
[0002] Non-oriented electrical steel sheets are mainly used as materials for the iron cores of rotating devices such as motors and generators, and stationary devices such as small transformers. Recently, as regulations for environmental conservation and energy saving have been strengthened, there has been an increasing demand for improved efficiency of motors and generators, which are energy conversion devices that convert electrical energy into mechanical energy and mechanical energy into electrical energy. Since non-oriented electrical steel sheets are used as materials for the iron cores of rotating devices such as motors and generators, and stationary devices such as small transformers, the demand for improved efficiency of motors and generators leads to a demand for improved properties of non-oriented electrical steel sheets.
[0003] The representative magnetic properties of non-oriented electrical steel sheets are iron loss and magnetic flux density. The lower the iron loss of non-oriented electrical steel sheets, the less iron loss occurs during the magnetization process of the iron core, improving efficiency. The higher the magnetic flux density, the stronger the magnetic field can be induced with the same energy, and less current can be applied to obtain the same magnetic flux density, improving energy efficiency. Therefore, in order to improve energy efficiency, it can be said that the development technology for non-oriented electrical steel sheets with low iron loss, high magnetic flux density, and excellent magnetism is essential.
[0004] Among the important properties of non-oriented electrical steel sheets, the most basic yet effective method for reducing iron loss is to increase the amount of Si, Al, and Mn, which are elements with high resistivity, or to reduce the thickness of the steel sheet. However, increasing the amount of Si, Al, and Mn added has the effect of reducing iron loss by increasing the resistivity of the steel and reducing the eddy current loss of the iron loss of non-oriented electrical steel sheets, but the effect varies depending on the addition ratio, and the magnetic flux density deteriorates as the amount of alloying elements added increases. Therefore, in order to ensure excellent iron loss and magnetic flux density, the appropriate addition amount and the addition ratio between the amounts of Si, Al, and Mn added must be properly controlled. Reducing the thickness is also very effective in reducing iron loss, but there is a disadvantage that a thin steel sheet reduces productivity and workability, resulting in a large increase in processing costs.
[0005] As a method for lowering the core loss of non-oriented electrical steel sheets and improving the magnetic flux density, some techniques have been reported, such as improving the texture by using special additive elements such as REM to improve the magnetic properties, or introducing additional manufacturing processes such as warm rolling, double rolling and double annealing. However, all of these techniques increase manufacturing costs and are difficult to mass-produce, so it is necessary to develop a technology that has excellent magnetic properties but is easy to produce commercially. In addition, a technology has been developed to suppress and control the formation of inclusions by minimizing the amount of added impurities and adding elements such as Ca, but this also increases manufacturing costs and it is not easy to clearly ensure its effectiveness.
[0006] There have been continuous efforts to solve these problems, and many technologies have been developed. Among the conventional technologies for non-oriented electrical steel sheets, a method was proposed in which the heating rate during final annealing was controlled to 50°C / s or more to improve the texture and ensure excellent magnetic properties, but apart from the result of improving the texture by performing rapid heating, the possibility of inferior magnetic properties due to the microstructure becoming non-uniform was not taken into consideration. In addition, in order to improve magnetic properties by improving the texture, a method was proposed in which the composition weight ratio (MnO / SiO2) of MnO and SiO2 in the oxide-based inclusions in the steel was adjusted, and finish rolling during hot rolling was performed in the ferrite single phase region where the friction coefficient between the steel and the roll was 0.2 or less and the finish rolling temperature was 700°C or more, followed by hot-rolled sheet annealing, cold rolling, and cold-rolled sheet annealing. However, this method has the limitation that the productivity is reduced and commercial production is difficult because the thickness of the hot-rolled sheet must be controlled to 1.0 mm or less.
[0007] Furthermore, in order to manufacture non-oriented electrical steel sheets with excellent magnetic properties in the rolling direction, a process of performing skin pass rolling at a rolling reduction rate of 3 to 10% and annealing again in addition to the processes of hot rolling, hot rolled sheet annealing, cold rolling, and cold rolled sheet annealing has been proposed. This also has the problem of increased costs due to the additional process. In addition, a method has been proposed in which a high-strength steel sheet is obtained before stress relief annealing and a steel sheet with low iron loss due to the ease of grain growth during annealing by reducing specific impurity elements to a very low level and adding a skin pass process, but there is a disadvantage in that costs increase due to the extremely low level of impurities. Furthermore, a technology has been proposed in which the precipitation of MnS is suppressed by adding rare earth elements such as Ca, Mg, and REM, and although the grains are small before stress relief, the grains grow during stress relief annealing, resulting in excellent iron loss. However, this also involves an increase in manufacturing costs due to the addition and control of additional elements, and if stress relief annealing is not performed, it is difficult to ensure the effect. Summary of the Invention [Problem to be solved by the invention]
[0008] An object of the present invention is to provide a non-oriented electrical steel sheet and a manufacturing method thereof. More specifically, an object of the present invention is to provide a non-oriented electrical steel sheet and a manufacturing method thereof in which As and P are appropriately added to improve the texture and magnetic properties. [Means for solving the problem]
[0009] A non-oriented electrical steel sheet according to one embodiment of the present invention contains, by weight, 2.5-4.0% Si, 0.1-1.0% Mn, 0.5-1.5% Al, 0.002-0.015% P, and 0.002-0.01% As, with the remainder being Fe and unavoidable impurities, and is characterized in that it satisfies the following formulas 1 and 2. [Formula 1] 0.005≦([P]+[As])≦0.015 (In formula 1, [P] and [As] represent the P and As contents (wt%), respectively.) [Formula 2] [STD]≦0.7×[GS] ([GS] is the average grain size (μm) measured when observing more than 10,000 grains having a grain size of 5 to 500 μm on the surface of the steel sheet, and STD indicates the standard deviation (μm) at that time.)
[0010] The non-oriented electrical steel sheet according to an embodiment of the present invention may further include one or more of C: 0.005 wt % or less, S: 0.005 wt % or less, N: 0.005 wt % or less, and Ti: 0.005 wt % or less.
[0011] The non-oriented electrical steel sheet according to an embodiment of the present invention may further include one or more of Sn: 0.2 wt % or less and Sb: 0.2 wt % or less.
[0012] The non-oriented electrical steel sheet according to an embodiment of the present invention may further include one or more of Cu: 0.05 wt.% or less, Ni: 0.05 wt.% or less, Cr: 0.05 wt.% or less, Zr: 0.01 wt.% or less, Mo: 0.01 wt.% or less, and V: 0.01 wt.% or less.
[0013] The non-oriented electrical steel sheet according to an embodiment of the present invention may have an average grain size ([GS]) of 90 to 200 μm.
[0014] The non-oriented electrical steel sheet according to an embodiment of the present invention may have a standard deviation ([STD]) of 60 to 100 μm.
[0015] The non-oriented electrical steel sheet according to an embodiment of the present invention may have a resistivity (ρ) of 60 μΩcm or more at room temperature.
[0016] The non-oriented electrical steel sheet according to an embodiment of the present invention may have an iron loss (W15 / 50) of 2.0 W / Kg or less.
[0017] The non-oriented electrical steel sheet according to one embodiment of the present invention can satisfy the following formulas 3 to 5. [Formula 3] Iron loss (W5 / 50) / Iron loss (W15 / 50)≦0.15 [Formula 4] Iron loss (W10 / 50) / Iron loss (W15 / 50)≦0.45 [Formula 5] Magnetic flux density (B1) / magnetic flux density (B50) ≧ 0.65
[0018] A method for producing a non-oriented electrical steel sheet according to one embodiment of the present invention is characterized in that it includes a step of hot rolling a slab containing, by weight, 2.5-4.0% Si, 0.1-1.0% Mn, 0.5-1.5% Al, 0.002-0.015% P, and 0.002-0.01% As, with the remainder being Fe and unavoidable impurities, and satisfying the following formula 1, to produce a hot-rolled sheet, a step of cold rolling the hot-rolled sheet to produce a cold-rolled sheet, and a step of final annealing the cold-rolled sheet. [Formula 1] 0.005≦([P]+[As])≦0.015 (In formula 1, [P] and [As] represent the P and As contents (wt%), respectively. In the final annealing stage, the tension on the annealing furnace entry side is 0.15 to 0.31 kgf / mm 2 The tension at the exit of the annealing furnace is 0.36 to 0.62 kgf / mm 2After the soaking, the cooling rate to 700° C. may be 30° C. / s or less during cooling.
[0019] At the final annealing stage, the difference (TS2-TS1) between the tension on the exit side of the annealing furnace (TS2) and the tension on the entry side of the annealing furnace (TS1) is 0.20 to 0.40 kgf / mm 2 may be also possible. Effect of the Invention
[0020] According to one embodiment of the present invention, a non-oriented electrical steel sheet having improved magnetic properties can be provided by appropriately adding As and P and improving the texture. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] Terms such as first, second and third are used to describe various parts, components, regions, layers and / or sections, but are not limited thereto. These terms are used only to distinguish one part, component, region, layer or section from another part, component, region, layer or section. Thus, a first part, component, region, layer or section described below may be referred to as a second part, component, region, layer or section without departing from the scope of the present invention.
[0022] The terminology used herein is merely for the purpose of referring to particular embodiments and is not intended to limit the present invention. As used herein, the singular form includes the plural form unless the text clearly indicates otherwise. The term "comprising" as used in the specification embodies certain features, regions, integers, steps, operations, elements and / or components and does not exclude the presence or addition of other features, regions, integers, steps, operations, elements and / or components.
[0023] When a part is said to be "on" another part, this means that it is exactly on top of the other part, or there may be other parts between them. In contrast, when a part is said to be "directly on" another part, there are no other parts between them. Also, unless otherwise specified, % means % by weight, and 1 ppm is 0.0001 wt. %. In one embodiment of the present invention, "further comprising an additional element" means that an additional amount of the additional element is included in place of the remaining iron (Fe).
[0024] Unless otherwise defined, all terms, including technical and scientific terms, used herein have the same meaning as commonly understood by a person of ordinary skill in the art to which the present invention belongs. Terms defined in commonly used dictionaries are additionally interpreted to have a meaning consistent with the relevant technical literature and the currently disclosed contents, and are not interpreted in an ideal or very formal sense unless otherwise defined. Hereinafter, embodiments of the present invention will be described in detail so that a person of ordinary skill in the art to which the present invention belongs can easily carry out the invention. However, the present invention may be realized in various different forms and is not limited to the embodiments described herein.
[0025] In one embodiment of the present invention, the important elements whose amounts and contents must be controlled are Si, Al, Mn, P, and As. The most efficient way to reduce iron loss is to increase the resistivity of steel by adding Si, Al, and Mn. However, when Si, Al, Mn, etc. are added to Fe, iron loss decreases, but the decrease in magnetic flux density due to the decrease in saturation magnetic flux density cannot be avoided, and in high alloy systems with a large amount of Si, Al, and Mn added, the cold rolling property is inferior due to the increase in brittleness of the material, making it difficult to ensure productivity. Therefore, in order to have low iron loss and high magnetic flux density properties and ensure productivity, an appropriate combination of the amounts and ratios of Si, Al, and Mn added is required. P is known as an element that can improve the texture and improve magnetism as a grain boundary and surface segregation element. According to the present invention, it has been confirmed that As can improve magnetism as a segregation element, like P. However, in the case of the above-mentioned segregation elements, the rollability deteriorates as the amount of addition increases, so the amount of addition must be appropriately controlled. In addition, when P and As are added in combination within a specified range, the effects are more reliably manifested. Therefore, from the viewpoints of magnetism and productivity, it is also necessary to control the amounts of these two elements within the specified ranges.
[0026] A non-oriented electrical steel sheet according to an embodiment of the present invention contains, by weight, 2.5-4.0% Si, 0.1-1.0% Mn, 0.5-1.5% Al, 0.002-0.015% P, and 0.002-0.01% As, with the remainder being Fe and unavoidable impurities.
[0027] The reasons for limiting the components of the non-oriented electrical steel sheet will be explained below.
[0028] Si:2.50~4.00wt% Silicon (Si) is a main element added to increase the resistivity of steel and reduce eddy current loss in iron loss. If too little Si is added, it may be difficult to obtain low iron loss characteristics. On the other hand, if too much Si is added, the magnetic flux density decreases significantly and production in a commercial process may become difficult due to increased brittleness. Therefore, Si may be contained at 2.5 to 4.0 wt %. More specifically, it may be contained at 2.7 to 3.9 wt %. Even more specifically, it may be contained at 2.9 to 3.7 wt %.
[0029] Mn:0.10~1.00wt% Manganese (Mn) is an element that, together with Si, Al, etc., increases resistivity and reduces core loss, and also improves texture. If too little Mn is added, fine sulfides may be formed. If too much Mn is added, magnetic flux density may be significantly reduced. Therefore, Mn may be contained in an amount of 0.10 to 1.00 wt %. More specifically, Mn may be contained in an amount of 0.20 to 0.95 wt %.
[0030] Al: 0.50~1.50% by weight Aluminum (Al) plays an important role in increasing resistivity together with Si to reduce core loss, and is also added to reduce magnetic anisotropy to reduce magnetic deviation in the rolling direction and the direction perpendicular to the rolling direction. If too little Al is added, the above-mentioned effects cannot be sufficiently obtained. Conversely, if too much Al is added, the magnetic flux density can be significantly reduced. Therefore, the Al content may be 0.50 to 1.50 wt %. More specifically, the Al content may be 0.60 to 1.30 wt %.
[0031] P:0.002~0.015wt% Phosphorus (P) is an element that segregates at grain boundaries and surfaces and has the effect of improving the texture of steel. If too little P is added, the above-mentioned effect cannot be obtained sufficiently. If too much P is added, the grain growth is suppressed due to the segregation effect, and the rolling property is deteriorated, which may decrease productivity. Therefore, P may be contained in an amount of 0.002 to 0.015% by weight. More specifically, P may be contained in an amount of 0.003 to 0.013% by weight.
[0032] As:0.002~0.010wt% Arsenic (As) is a grain boundary and surface segregation element, like P, and has the effect of improving the texture of steel. If too little As is added, the above-mentioned effect cannot be obtained sufficiently. If too much As is added, grain growth is suppressed, and rollability is deteriorated, which may reduce productivity. Therefore, As may be contained in an amount of 0.002 to 0.010% by weight. More specifically, As may be contained in an amount of 0.002 to 0.009% by weight.
[0033] In one embodiment of the present invention, P and As satisfy the following formula 1. [Formula 1] 0.005≦([P]+[As])≦0.015 (In formula 1, [P] and [As] represent the P and As contents (wt%), respectively.)
[0034] P and As are elements that improve magnetic properties by reducing the {111} texture, which is detrimental to magnetic properties in the texture during the recrystallization process of steel, by segregating at grain boundaries and surfaces. However, the cold rollability of steel deteriorates as the amount of addition increases, so the amount must be limited to a certain range. Additionally, in one embodiment of the present invention, it has been confirmed that the magnetic improvement effect is greater when P and As are added in combination, and as a result of investigating the range of the appropriate amount of addition, it has been confirmed that the effect can be secured when the P and As satisfy the formula 1. More specifically, the value of formula 1 may be 0.006 to 0.015.
[0035] The non-oriented electrical steel sheet according to an embodiment of the present invention may further include one or more of C: 0.005 wt % or less, S: 0.005 wt % or less, N: 0.005 wt % or less, and Ti: 0.005 wt % or less.
[0036] C: 0.005% by weight or less Carbon (C) combines with Ti, Nb, etc. to form carbides, which impairs magnetic properties, and when processed into an electrical product from the final product, magnetic aging increases core loss during use, reducing the efficiency of the electrical device, so it may be contained in an amount of 0.005% by weight or less, more specifically, 0.003% by weight or less.
[0037] S: 0.005% by weight or less Sulfur (S) is an element that forms sulfides such as MnS, CuS, and (Cu, Mn)S, which are harmful to magnetic properties, so it can be added in as small an amount as possible. Therefore, the upper limit can be limited to 0.005% by weight. If S is contained in an excessively small amount, it is rather disadvantageous to the formation of the texture, and the formation of fine sulfides can be promoted, which can reduce magnetic properties, so it is also possible to add 0.001% by weight or more. In other words, if S is further contained, it can be added in an amount of 0.005% by weight or less, more specifically, 0.001 to 0.005% by weight.
[0038] N: 0.005% by weight or less Nitrogen (N) is an element that is harmful to magnetism, for example by forming nitrides by strongly bonding with Al, Ti, Nb, etc., and inhibiting grain growth, so it can be contained in small amounts. Therefore, when N is further contained, it can be contained in an amount of 0.005% by weight or less. More specifically, it can be contained in an amount of 0.003% by weight or less.
[0039] Ti: 0.005% by weight or less Titanium (Ti) forms fine carbides and nitrides by combining with C and N, suppressing grain growth, and the more Ti is added, the more carbides and nitrides there are, leading to poor texture and poor magnetic properties. Therefore, if Ti is further added, it should be limited to 0.005% by weight or less. More specifically, it can be contained in an amount of 0.003% by weight or less.
[0040] The non-oriented electrical steel sheet according to an embodiment of the present invention may further include one or more of Sn: 0.2 wt % or less and Sb: 0.2 wt % or less. Sn and Sb have the effect of improving the texture and can be added to further improve magnetic properties, but if the amount added is too large, it can inhibit grain growth and reduce productivity, so the amount added can be limited to 0.2 wt % or less.
[0041] In the case of Cu, Ni, and Cr, they react with impurity elements to form fine sulfides, carbides, and nitrides, which have a detrimental effect on magnetic properties, so their contents are limited to 0.05% by weight or less. In addition, Zr, Mo, V, and other elements are also strong carbonitride-forming elements, so it is preferable to avoid adding them as much as possible, and each is contained at 0.01% by weight or less.
[0042] The balance includes Fe and inevitable impurities. The inevitable impurities are impurities that are mixed in during the steelmaking stage and the manufacturing process of the grain-oriented electrical steel sheet, and are widely known in the art, so a detailed description will be omitted. In one embodiment of the present invention, the addition of elements other than the above-mentioned alloy components is not excluded, and various elements are included within a range that does not impair the technical concept of the present invention. When an additional element is further included, it is included in place of the balance Fe.
[0043] The unavoidable impurities include, for example, B and Mg, and must be controlled to B: 0.002% by weight or less, and Mg: 0.005% by weight or less. In one embodiment of the present invention, the crystal grains satisfy the following formula 2. [Formula 2] [STD]≦0.7×[GS] ([GS] is the average grain size (μm) measured when observing more than 10,000 grains having a grain size of 5 to 500 μm on the surface of the steel sheet, and STD indicates the standard deviation (μm) at that time.)
[0044] Formula 2 means that the grain size is distributed close to the average. However, as the grain size becomes larger, the distribution becomes more distant, and the standard deviation is limited in proportion to the grain size. When the value of formula 2 is not satisfied, it means that the deviation of the grain size is large, and ultimately the magnetic property is poor. More specifically, 0.60 x [GS] ≦ [STD] ≦ 0.68 x [GS] must be satisfied.
[0045] Specifically, the standard deviation (STD) may be a population standard deviation. More specifically, it is calculated for n crystal grains by the following formula: TIFF0007594590000001.tif27128Gs i is the grain size of the i-th grain, and Gs is the average grain size.
[0046] The non-oriented electrical steel sheet according to an embodiment of the present invention may have an average crystal grain size ([GS]) of 90 to 200 μm. Within the above-mentioned range, the magnetic properties are further improved. Furthermore, the non-oriented electrical steel sheet according to an embodiment of the present invention may have a standard deviation ([STD]) of 60 to 100 μm. Within the above-mentioned range, the magnetic properties are further improved. The grain size of the crystal grains is determined based on the plate surface (ND surface), and a virtual circle with the same area as the crystal grain is assumed, and the diameter of the circle is taken as the grain size. Specifically, the non-oriented electrical steel sheet according to an embodiment of the present invention may have an iron loss (W15 / 50) of 2.0 W / Kg or less.
[0047] Furthermore, the non-oriented electrical steel sheet according to one embodiment of the present invention can satisfy the following formulas 3 to 5. [Formula 3] Iron loss (W5 / 50) / Iron loss (W15 / 50)≦0.15 [Formula 4] Iron loss (W10 / 50) / Iron loss (W15 / 50)≦0.45 [Formula 5] Magnetic flux density (B1) / magnetic flux density (B50) ≧ 0.65
[0048] Iron loss (W 5 / 50 ) is the iron loss when a magnetic flux density of 0.5T is induced at a frequency of 50Hz. Iron loss (W 10 / 50 ) is the iron loss when a magnetic flux density of 1.0T is induced at a frequency of 50Hz. Iron loss (W 15 / 50 ) is the iron loss when a magnetic flux density of 1.5T is induced at a frequency of 50Hz. Magnetic flux density (B1) is the magnetic flux density induced in a magnetic field of 100A / m. Magnetic flux density (B 50 ) is the magnetic flux density induced in a magnetic field of 5000 A / m. By satisfying formulas 3 to 5, when used as a motor material, it does not only show excellent characteristics in a specific frequency and magnetic field region, but also shows consistently excellent efficiency even when the frequency and magnetic field change.
[0049] A method for manufacturing a non-oriented electrical steel sheet according to an embodiment of the present invention includes the steps of hot rolling a slab to manufacture a hot-rolled sheet, cold rolling the hot-rolled sheet to manufacture a cold-rolled sheet, and final annealing the cold-rolled sheet. First, the slab is hot-rolled. The alloy components of the slab have been described above in relation to the alloy components of the non-oriented electrical steel sheet, and therefore will not be described again here. Since the alloy components do not substantially vary during the manufacturing process of the non-oriented electrical steel sheet, the alloy components of the non-oriented electrical steel sheet and the slab are substantially the same.
[0050] Specifically, the slab contains, by weight, 2.5-4.0% Si, 0.1-1.0% Mn, 0.5-1.5% Al, 0.002-0.015% P, and 0.002-0.01% As, with the balance being Fe and unavoidable impurities, and satisfies the following formula 1. Other additional elements have been explained in the alloy components of non-oriented electrical steel sheets, so duplicate explanations will be omitted. The slab can be heated before hot rolling. The heating temperature of the slab is not limited, but the slab can be heated to 1200°C or less. If the heating temperature of the slab is excessively high, precipitates such as nitrides, carbides, and sulfides present in the slab may be redissolved and then finely precipitate during hot rolling and annealing, suppressing grain growth and reducing magnetism.
[0051] The thickness of the hot-rolled sheet may be 2 to 2.3 mm. In the step of producing the hot-rolled sheet, the finish rolling temperature may be 800° C. or more. Specifically, it may be 800 to 1000° C. The hot-rolled sheet is coiled at a temperature of 700° C. or less. After the step of producing the hot-rolled sheet, the method may further include a step of annealing the hot-rolled sheet. At this time, the annealing temperature of the hot-rolled sheet may be 950 to 1150° C. If the annealing temperature of the hot-rolled sheet is too low, the structure does not grow or grows finely, and it is not easy to obtain a texture advantageous for magnetic properties during annealing after cold rolling. If the annealing temperature is too high, the crystal grains grow excessively, and the surface defects of the sheet may become excessive. The hot-rolled sheet annealing is performed to increase the orientation advantageous for magnetic properties as necessary, and may be omitted. The annealed hot-rolled sheet may be pickled.
[0052] Next, the hot rolled sheet is cold rolled to produce a cold rolled sheet. The cold rolling is final rolling to a thickness of 0.10 mm to 0.50 mm. If necessary, the cold rolling step may include one cold rolling step or two or more cold rolling steps with intermediate annealing in between. In this case, the intermediate annealing temperature may be 850 to 1150°C. In the cold rolling step, the final reduction may be adjusted to 50% to 95%.
[0053] Next, the cold-rolled sheet is subjected to final annealing. In the process of annealing the cold-rolled sheet, the annealing temperature is not significantly limited as long as it is a temperature that is generally applied to non-oriented electrical steel sheets. The iron loss of non-oriented electrical steel sheets is closely related to the size of the crystal grains. The iron loss of non-oriented electrical steel sheets can be divided into hysteresis loss and eddy current loss. The hysteresis loss decreases as the grain size of the crystal grains increases, and conversely, the eddy current loss increases as the grain size increases, and there is an appropriate grain size at which the sum of the hysteresis loss and the eddy current loss is minimized. Therefore, from a macroscopic point of view, it is important to derive and apply an annealing temperature that can ensure the optimal grain size, and an annealing temperature of 900 to 1100 ° C is appropriate. If the temperature is too low, the crystal grains may be too fine and the hysteresis loss may increase. If the temperature is too high, the crystal grains may be too coarse and the eddy current loss may increase, resulting in poor iron loss. However, from a microscopic point of view, even if the crystal grain size is the same, the more uniform the microstructure, the better the iron loss. Even if the average grain size is similar, if the standard deviation is large, the iron loss is deteriorated, so in order to ensure uniformity of the microstructure, it was confirmed that excellent magnetic properties can be obtained by controlling the cooling rate to 700°C after reaching a maximum temperature in the range of 900 to 1100°C during cold-rolled sheet annealing so as to be 30°C / s or less during cooling. More specifically, the cooling rate may be 15 to 30°C / s.
[0054] In addition, in one embodiment of the present invention, it was confirmed that another important control factor during final annealing is the annealing tension at the inlet and outlet of the annealing furnace. When the annealing tension is high, residual stress remains in the sheet and deteriorates the magnetic property, but it does not significantly affect the magnetic property in the high magnetic field region, but in the low magnetic field region, the magnetic property is significantly deteriorated depending on the residual stress. Not only the characteristics in the high magnetic field region but also the characteristics in the low magnetic field region are important, but generally there is a tendency to check the characteristics in the high magnetic field region and not the low magnetic field region. However, when used as a motor material, not only the characteristics in the high magnetic field region but also the characteristics in the low magnetic field region are important for the efficiency of the motor, so it is necessary to improve the characteristics in the low magnetic field region as well.
[0055] For this reason, the tension on the annealing furnace entry side is set to 0.15 to 0.31 kgf / mm 2The tension at the exit of the annealing furnace is 0.36 to 0.62 kgf / mm 2 When the tension difference (TS2-TS1) between the exit tension (TS2) of the annealing furnace and the entry tension (TS1) of the annealing furnace is 0.20 to 0.40 kgf / mm, the residual stress can be reduced and the properties can be improved not only in high magnetic fields but also in low magnetic fields. 2 When the content is adjusted to the above range, the above-mentioned effects can be further improved. After the final annealing, an insulating coating can be formed. The insulating coating can be an organic, inorganic or organic-inorganic composite coating, and can also be a coating agent capable of providing other insulation.
[0056] The present invention will be described in more detail with reference to the following examples, which are merely for illustrative purposes and are not intended to limit the scope of the present invention. EXAMPLES
[0057] A slab was produced with the ingredients shown in Tables 1 and 2, with the balance being Fe and unavoidable impurities. It was heated to 1180°C and hot rolled to produce a hot rolled sheet with a thickness of 2.3 mm. The hot rolled sheet was annealed at 1000°C and pickled. Thereafter, the hot rolled sheet was cold rolled to a thickness of 0.35 mm and subjected to final annealing. The final annealing temperature is summarized in Table 2 below, and the tension on the annealing furnace entry side was 0.25 kgf / mm 2 , the tension on the exit side is 0.55kgf / mm 2 After annealing at the maximum temperature, the cooling rate was 25°C / s down to 700°C. The microstructure of each test piece was observed to analyze the grain size, and the iron losses W5 / 50, W10 / 50, and W15 / 50 and magnetic flux densities B1 and B50 were measured by Epstein sample processing. The results are shown in Tables 2 and 3 below.
[0058] [Table 1]
[0059] [Table 2]
[0060] [Table 3]
[0061] As shown in Tables 1 to 3, after final annealing of A1, A4, A5, A7, A8, and A10 in which the alloy components and [STD] / [GS] factors were appropriately controlled, the iron loss (W15 / 50) was 2.0 W / Kg or less, and the iron loss relationship equations of iron loss (W5 / 50) / iron loss (W15 / 50)≦0.15 and iron loss (W10 / 50) / iron loss (W15 / 50)≦0.45 and the magnetic flux density relationship equation of magnetic flux density (B1) / magnetic flux density (B50)≧0.65 were all satisfied, and they showed very good magnetic properties. In contrast, A2 contained excessive Mn and little Al, and as a result, it was found to be inferior to W15 / 50 and B50 in terms of iron loss. A3 contained little Si, and as a result, it was found to be inferior to W15 / 50 and B50 in terms of iron loss. A6 contained excessive As, did not satisfy [P] + [As], did not satisfy the [STD] / [GS] range, and as a result, was found to be inferior to W15 / 50 and B50 in iron loss. A9 did not satisfy [P] + [As], did not satisfy the [STD] / [GS] range, and as a result, was found to be inferior to W15 / 50 and B50 in iron loss. A11 contained excessively little P and As, and was found to be inferior to W15 / 50 and B50 in iron loss. EXAMPLES
[0062] Slabs were produced from the components shown in Tables 4 and 5, with the balance being Fe and unavoidable impurities. These were heated to 1160°C and hot-rolled to produce hot-rolled sheets with a thickness of 2.1 mm. The hot-rolled sheets were annealed at 1020°C and pickled. The hot-rolled sheets were then cold-rolled to a thickness of 0.35 mm and subjected to final annealing. The final annealing temperature, the tension at the annealing furnace entrance side, the tension at the annealing furnace exit side, and the cooling rate to 700°C after annealing at the maximum temperature are summarized in Table 5 below. The microstructure of each test piece was observed to analyze the grain size, and the iron losses W5 / 50, W10 / 50, and W15 / 50 and the magnetic flux densities B1 and B50 were measured by Epstein sample processing, and the results are shown in Tables 5 and 6 below.
[0063] [Table 4]
[0064] [Table 5]
[0065] [Table 6]
[0066] As shown in Tables 4 to 6, B1, B3, B4, B5, B8, and B10, which satisfied all of the alloy components, manufacturing process conditions, and grain size characteristics, had an iron loss (W15 / 50) of 2.0 W / Kg or less after final annealing, and also satisfied the iron loss relationship equations of iron loss (W5 / 50) / iron loss (W15 / 50)≦0.15 and iron loss (W10 / 50) / iron loss (W15 / 50)≦0.45, as well as the magnetic flux density relationship equation of magnetic flux density (B1) / magnetic flux density (B50)≧0.65, showing extremely excellent magnetic properties.
[0067] In contrast, B2 did not satisfy the tension conditions on the inlet side of the annealing furnace, the tension conditions on the outlet side, and the cooling rate conditions, and therefore [STD] / [GS] could not be properly formed. As a result, not only did it not satisfy the iron loss relationship equations of iron loss (W5 / 50) / iron loss (W15 / 50) ≦ 0.15 and iron loss (W10 / 50) / iron loss (W15 / 50) ≦ 0.45, and the magnetic flux density relationship equation of magnetic flux density (B1) / magnetic flux density (B50) ≧ 0.65, but it was also found that the iron loss W15 / 50 and magnetic flux density B50 were inferior. B6 does not satisfy the P composition, [P] + [As], and does not satisfy the tension and cooling rate on the annealing furnace entry side, so [STD] / [GS] cannot be properly formed. Not only does it not satisfy the iron loss relationship equations of iron loss (W5 / 50) / iron loss (W15 / 50) ≦ 0.15 and iron loss (W10 / 50) / iron loss (W15 / 50) ≦ 0.45, and the magnetic flux density relationship equation of magnetic flux density (B1) / magnetic flux density (B50) ≧ 0.65, but it was also found that the iron loss W15 / 50 and magnetic flux density B50 are inferior.
[0068] B7 did not satisfy [P]+[As], and was out of the range of tension on the inlet side and outlet side of the annealing furnace, and did not satisfy the iron loss relationship equations of iron loss (W5 / 50) / iron loss (W15 / 50)≦0.15 and iron loss (W10 / 50) / iron loss (W15 / 50)≦0.45, and the magnetic flux density relationship equation of magnetic flux density (B1) / magnetic flux density (B50)≧0.65. It was also found that the iron loss W15 / 50 and magnetic flux density B50 were inferior. B9 did not satisfy the tension and cooling rate on the outlet side of the annealing furnace, and as a result, [STD] / [GS] could not be formed properly. As a result, it was found that the iron loss relationship equations of iron loss (W5 / 50) / iron loss (W15 / 50) ≦ 0.15 and iron loss (W10 / 50) / iron loss (W15 / 50) ≦ 0.45, and the magnetic flux density relationship equation of magnetic flux density (B1) / magnetic flux density (B50) ≧ 0.65 were not satisfied, and it was found that the iron loss W15 / 50 and magnetic flux density B50 were also inferior.
[0069] On the other hand, B11 does not satisfy the As content range and [P] + [As], and does not satisfy the tension and cooling rate at the exit of the annealing furnace, so [STD] / [GS] cannot be properly formed, and not only does it not satisfy the iron loss relationship equation of iron loss (W5 / 50) / iron loss (W15 / 50) ≦ 0.15 and iron loss (W10 / 50) / iron loss (W15 / 50) ≦ 0.45, and the magnetic flux density relationship equation of magnetic flux density (B1) / magnetic flux density (B50) ≧ 0.65, but it was also found that the iron loss W15 / 50 and magnetic flux density B50 were inferior. Finally, B12 does not satisfy the tension and cooling rate at the entrance of the annealing furnace, so that [STD] / [GS] cannot be properly formed. As a result, it was found that the iron loss relationship equations of iron loss (W5 / 50) / iron loss (W15 / 50) ≦ 0.15 and iron loss (W10 / 50) / iron loss (W15 / 50) ≦ 0.45, and the magnetic flux density relationship equation of magnetic flux density (B1) / magnetic flux density (B50) ≧ 0.65 were not satisfied, and it was found that the iron loss W15 / 50 and magnetic flux density B50 were also inferior.
[0070] The present invention is not limited to the above-mentioned embodiments, and can be manufactured in various different forms, and a person skilled in the art to which the present invention pertains will understand that the present invention can be embodied in other specific forms without changing the technical concept or essential features of the present invention. Therefore, it should be understood that the above-mentioned embodiments are illustrative in all respects and not limiting.
Claims
1. A non-oriented electrical steel sheet comprising, by weight, 2.5-4.0% Si, 0.1-1.0% Mn, 0.5-1.5% Al, 0.002-0.015% P, and 0.002-0.01% As, with the balance being Fe and unavoidable impurities, and satisfying the following formulas 1 and 2; and an average crystal grain size ([GS]) of 90-200 μm. [Formula 1] 0.005≦([P]+[As])≦0.015 (In formula 1, [P] and [As] represent the contents (wt%) of P and As, respectively.) [Formula 2] 60≦[STD]≦0.70×[GS] ([GS] is the average grain size (μm) measured when observing 10,000 or more grains having a grain size of 5 to 500 μm on the surface of the steel sheet, and STD indicates the standard deviation (μm) at that time.)
2. 2. The non-oriented electrical steel sheet according to claim 1, further comprising one or more of C: 0.005 wt % or less, S: 0.005 wt % or less, N: 0.005 wt % or less, and Ti: 0.005 wt % or less.
3. The non-oriented electrical steel sheet according to claim 1 or 2, characterized in that the standard deviation ([STD]) is 60 to 100 μm.
4. The non-oriented electrical steel sheet according to any one of claims 1 to 3, characterized in that the resistivity (ρ) at room temperature is 60 μΩcm or more.
5. The non-oriented electrical steel sheet according to any one of claims 1 to 4, characterized in that the core loss (W15 / 50) is 2.0 W / Kg or less.
6. The non-oriented electrical steel sheet according to any one of claims 1 to 5, characterized in that the following formulas 3 to 5 are satisfied: [Formula 3] Iron loss (W5 / 50) / Iron loss (W15 / 50)≦0.15 [Formula 4] Iron loss (W10 / 50) / Iron loss (W15 / 50)≦0.45 [Formula 5] Magnetic flux density (B1) / magnetic flux density (B50)≧0.65
7. A step of producing a hot-rolled sheet by hot rolling a slab containing, by weight, 2.5 to 4.0% Si, 0.1 to 1.0% Mn, 0.5 to 1.5% Al, 0.002 to 0.015% P, and 0.002 to 0.01% As, with the balance being Fe and unavoidable impurities, and satisfying the following formula 1: cold rolling the hot rolled sheet to produce a cold rolled sheet; and final annealing of the cold rolled sheet; In the final annealing step, the tension on the annealing furnace entry side is 0.15 to 0.31 kgf / mm 2 The tension at the exit side of the annealing furnace is 0.36 to 0.62 kgf / mm 2 After the soaking, the cooling rate to 700° C. is 30° C. / s or less during cooling; The produced non-oriented electrical steel sheet has an average grain size ([GS]) of 90 to 200 μm, A method for producing a non-oriented electrical steel sheet, characterized in that the following formula 2 is satisfied: [Formula 1] 0.005≦([P]+[As])≦0.015 (In formula 1, [P] and [As] represent the contents (wt%) of P and As, respectively.) [Formula 2] 60≦[STD]≦0.70×[GS] ([GS] is the average grain size (μm) measured when observing 10,000 or more grains having a grain size of 5 to 500 μm on the surface of the steel sheet, and STD indicates the standard deviation (μm) at that time.)
8. The difference (TS2-TS1) between the tension on the exit side of the annealing furnace (TS2) and the tension on the entry side of the annealing furnace (TS1) is 0.20 to 0.40 kgf / mm 2 The method for producing a non-oriented electrical steel sheet according to claim 7,
Citation Information
Patent Citations
Continuous annealing method for non-oriented silicon steel sheet
JP1989234524A
Non-oriented magnetic steel sheet and production method therefor
JP2012036455A
Non-oriented electromagnetic steel sheet, and method of producing the same
JP2013044010A
Nonoriented electromagnetic steel sheet having reduced deterioration in core loss caused by punching method
JP2014040622A
Nonoriented magnetic steel sheet, and method of producing the same
JP2019026891A