Non-oriented electrical steel sheet and its manufacturing method
By controlling Al, Mn, Cu, Ti, S, and N in non-oriented electrical steel sheets and forming a dense oxide layer, the steel sheets achieve improved magnetic properties and reduced iron loss, addressing manufacturing challenges and enhancing motor efficiency.
Patent Information
- Application Number
- JP2022537614
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-12-20
- Filing Date
- 2020-12-09
- Publication Date
- 2024-12-04
- Estimated Expiration
- 2040-12-09
AI Technical Summary
Existing non-oriented electrical steel sheets face challenges in achieving high magnetic properties, particularly at high frequencies and low magnetic fields, due to issues with alloy element additions affecting resistivity, brittleness, and surface characteristics, leading to increased manufacturing costs and reduced productivity.
A non-oriented electrical steel sheet with controlled amounts of Al, Mn, Cu, Ti, S, and N, forming a dense Al-based oxide layer on the surface to suppress AlN precipitates, optimized through specific alloy composition and annealing conditions.
The solution results in improved magnetic properties with reduced iron loss and increased magnetic flux density, enhancing motor efficiency and productivity by suppressing AlN precipitates and forming a dense oxide layer.
Smart Images

Figure 0007594592000004 
Figure 0007594592000001 
Figure 0007594592000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a non-oriented electrical steel sheet and a manufacturing method thereof, and more particularly to a non-oriented electrical steel sheet having improved magnetic properties by appropriately controlling the quantitative relationships between Al, Mn, Cu, Ti, S, and N and suppressing the formation of AlN precipitates in the surface layer of a base material, and a manufacturing method thereof. [Background technology]
[0002] Non-oriented electrical steel sheets are mainly used in motors that convert electrical energy into mechanical energy, and the excellent magnetic properties of non-oriented electrical steel sheets are required to achieve high efficiency in the conversion process. In recent years, environmentally friendly technologies have been attracting attention in particular, and great importance has been placed on improving the efficiency of motors, which account for more than half of the total electrical energy consumption, and as a result, the demand for non-oriented electrical steel sheets with excellent magnetic properties is also increasing. The magnetic properties of non-oriented electrical steel sheets are mainly evaluated by iron loss and magnetic flux density. Iron loss refers to the energy loss that occurs at a specific magnetic flux density and frequency, while magnetic flux density refers to the degree of magnetization obtained under a specific magnetic field. The lower the iron loss, the more energy-efficient a motor can be manufactured under the same conditions, and the higher the magnetic flux density, the more compact the motor can be and the less copper loss it can be. Therefore, it is important to create non-oriented electrical steel sheets with low iron loss and high magnetic flux density.
[0003] The characteristics of non-oriented electrical steel sheets that must be considered vary depending on the operating conditions of the motor. The iron loss (W) of many motors when a commercial frequency of 50 Hz and a magnetic field of 1.5 T are applied is used as a standard for evaluating the characteristics of non-oriented electrical steel sheets used in motors. 15 / 50 However, all motors for various applications are W 15 / 50 Iron loss is not the most important factor, but iron loss is also evaluated at other frequencies and applied magnetic fields depending on the main operating conditions. In particular, for non-oriented electrical steel sheets with a thickness of 0.35 mm or less used in the drive motors of recent electric vehicles, magnetic properties at low magnetic fields of 1.0 T or less and high frequencies of 400 Hz or more are often important, so W 10 / 400The characteristics of non-oriented electrical steel sheets are now being evaluated using iron loss such as The usual method for improving the magnetic properties of non-oriented electrical steel sheets is to add alloying elements such as Si. The addition of such alloying elements can increase the resistivity of the steel, and the higher the resistivity, the lower the eddy current loss and the lower the overall iron loss. On the other hand, the more Si added, the lower the magnetic flux density and the greater the brittleness. If more than a certain amount is added, cold rolling becomes difficult and commercial production becomes impossible. In particular, with electrical steel sheets, the thinner the thickness, the lower the iron loss, but the lower rollability due to brittleness becomes a fatal problem. Meanwhile, attempts have been made to add elements other than Si, such as Al and Mn, to increase the resistivity of the steel.
[0004] For non-oriented electrical steel sheets used in electric vehicle drive motors, iron loss at high frequencies of 400 Hz or more is important, but as the frequency increases, the ratio of eddy current loss to iron loss increases, so it is advantageous to increase resistivity and reduce thickness. However, as mentioned above, increasing the amount of elements added to increase resistivity reduces rollability, so increasing resistivity while reducing thickness inevitably reduces productivity in rolling and continuous annealing. Research has been conducted to improve this, such as adding specific elements or increasing the rolling temperature, but these have not been applied to commercial production due to rising manufacturing costs and lack of effectiveness.
[0005] When the operating frequency increases, as in the case of electric vehicle drive motors, a phenomenon occurs in which current concentrates on the surface of the steel sheet due to the skin effect. Therefore, the characteristics of the steel sheet surface have a very important impact on improving high-frequency characteristics. Research has been conducted into silicon deposition and diffusion to improve surface roughness through physicochemical methods in order to improve surface resistivity, but not only is it difficult to achieve using existing process equipment, but the effects are either small or the manufacturing costs rise significantly, greatly limiting the fields of application. Summary of the Invention [Problem to be solved by the invention]
[0006] The object of the present invention is to provide a non-oriented electrical steel sheet and a manufacturing method thereof, specifically, a non-oriented electrical steel sheet and a manufacturing method thereof in which the quantitative relationship between Al, Mn, Cu, Ti, S, and N is appropriately controlled to suppress the formation of AlN precipitates and improve magnetic properties, and a manufacturing method thereof. [Means for solving the problem]
[0007] The non-oriented electrical steel sheet of the present invention contains, by weight, 1.5 to 4.0% Si, 0.5 to 1.5% Al, 0.05 to 0.55% Mn, 0.005% or less C, 0.004% or less (excluding 0%) Ti, 0.005% or less (excluding 0%) N, 0.005% or less (excluding 0%) S, 0.01% or less Cu (excluding 0%), with the balance being Fe and unavoidable impurities, and satisfies the following formulas 1 and 2: The electrical steel sheet includes an oxide layer extending from the surface toward the inside, the oxide layer containing 50% by weight or more of Al, and the oxide layer having a thickness of 10 to 50 nm. [Formula 1] [N]≦0.005×([Al]+[Ti]) [Formula 2] [S]≦0.01×([Mn]+[Cu]) (In formulas 1 and 2, [N], [Al], [Ti], [S], [Mn] and [Cu] represent the contents (wt%) of N, Al, Ti, S, Mn and Cu, respectively.)
[0008] One or more of Nb and V may further be contained in an amount of up to 0.004% by weight each. One or more of Cr and Ni may further be contained in an amount of 0.05% by weight or less each. One or more of Sn and Sb may further be contained in an amount of 0.1% by weight or less each.
[0009] It may further contain one or more of P: 0.02% by weight or less, B: 0.002% by weight or less, Mg: 0.005% by weight or less, and Zr: 0.005% by weight or less. The number of AlN precipitates with a diameter of 100 nm or less in a cross section from the surface to a depth of 20 μm was 0.1 / mm 2 It is preferable that: The average crystal grain size is preferably 50 to 100 μm.
[0010] The method for producing a non-oriented electrical steel sheet of the present invention includes the steps of hot rolling a slab which is, by weight, 1.5 to 4.0% Si, 0.5 to 1.5% Al, 0.05 to 0.55% Mn, 0.005% or less C, 0.004% or less (excluding 0%) Ti, 0.005% or less (excluding 0%) N, 0.005% or less (excluding 0%) S, 0.005% or less (excluding 0%) Cu, with the balance being Fe and unavoidable impurities, and which satisfies the following formulas 1 and 2 to produce a hot-rolled sheet, cold rolling the hot-rolled sheet to produce a cold-rolled sheet, final annealing the cold-rolled sheet, and cooling the final annealed cold-rolled sheet, and is characterized in that in the step of cooling the final annealed cold-rolled sheet, the time for exposure to an atmosphere having a temperature of 700°C or less and a dew point exceeding 0°C is 5 to 20 seconds. [Formula 1] [N]≦0.005×([Al]+[Ti]) [Formula 2] [S]≦0.01×([Mn]+[Cu]) (In formulas 1 and 2, [N], [Al], [Ti], [S], [Mn] and [Cu] represent the contents (wt%) of N, Al, Ti, S, Mn and Cu, respectively.)
[0011] Preferably, the method further comprises a step of heating the slab at a temperature of 1200° C. or less prior to the step of producing the hot rolled sheet. In the hot rolling stage, the finish rolling temperature is preferably 800° C. or higher. After the hot rolling step, the method may further include a step of annealing the hot rolled sheet at a temperature in the range of 850 to 1150°C. The final annealing step preferably further comprises a step of annealing in a non-oxidizing atmosphere at a temperature of 700 to 1050° C. for 50 to 90 seconds. The non-oxidizing atmosphere preferably contains 5% by volume or more of H2 and has a dew point of 0°C or less. Effect of the Invention
[0012] According to one embodiment of the present invention, by identifying the optimal alloy composition of a non-oriented electrical steel sheet and presenting cooling conditions after annealing, it is possible to form a dense Al-based oxide layer on the surface of the electrical steel sheet and suppress the formation of fine AlN precipitates. Furthermore, according to one embodiment of the present invention, by providing a non-oriented electrical steel sheet with excellent magnetic properties, it is possible to contribute to improving the efficiency of motors and generators. [Brief description of the drawings]
[0013] [Figure 1] FIG. 1 is a schematic diagram of a cross section of a non-oriented electrical steel sheet according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] Terms such as first, second and third are used to describe various parts, components, regions, layers and / or sections, but are not limited thereto. These terms are used only to distinguish one part, component, region, layer or section from another part, component, region, layer or section. Thus, the first part, component, region, layer or section described below may be referred to as the second part, component, region, layer or section without departing from the scope of the present invention. The terminology used herein is merely for the purpose of referring to particular embodiments and is not intended to limit the present invention. As used herein, the singular form includes the plural form unless the text clearly indicates otherwise. The meaning of "comprising" as used in the specification embodies certain features, regions, integers, steps, operations, elements and / or components and does not exclude the presence or addition of other features, regions, integers, steps, operations, elements and / or components.
[0015] When an element is referred to as being "on" another element, it means that it is immediately on top of the other element, or there may be other elements between them. In contrast, when an element is referred to as being "directly on" another element, there are no other elements between them. Moreover, unless otherwise specified, % means % by weight, and 1 ppm is 0.0001% by weight. In an embodiment of the present invention, the term "additionally contain an additional element" means that the additional element is included in place of the remaining iron (Fe) by an amount corresponding to the additional element. Unless otherwise defined, all terms, including technical and scientific terms, used herein have the same meaning as commonly understood by a person of ordinary skill in the art to which the present invention belongs. Terms defined in commonly used dictionaries are additionally interpreted to have a meaning consistent with the relevant technical literature and the presently disclosed content, and are not interpreted in an ideal or very formal sense unless defined. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will now be described in detail with reference to exemplary embodiments thereof, so that those skilled in the art will be able to easily practice the present invention. However, the present invention may be embodied in many different forms and is not limited to the embodiments set forth herein.
[0016] A non-oriented electrical steel sheet according to one embodiment of the present invention contains, by weight, 1.5-4.0% Si, 0.5-1.5% Al, 0.05-0.55% Mn, 0.005% or less C, 0.004% or less (excluding 0%) Ti, 0.005% or less (excluding 0%) N, 0.005% or less (excluding 0%) S, and 0.01% or less (excluding 0%) Cu, with the remainder being Fe and unavoidable impurities, and satisfies the following formulas 1 and 2. [Formula 1] [N]≦0.005×([Al]+[Ti]) [Formula 2] [S]≦0.01×([Mn]+[Cu]) (In formulas 1 and 2, [N], [Al], [Ti], [S], [Mn] and [Cu] represent the contents (wt%) of N, Al, Ti, S, Mn and Cu, respectively.) The reasons for limiting the composition of non-oriented electrical steel sheets are explained below.
[0017] Si:1.5~4.0wt% Silicon (Si) is a main element added to increase the resistivity of steel and reduce eddy current loss in iron loss. If too little Si is added, the iron loss cannot be suppressed. Conversely, if too much Si is added, the magnetic flux density is significantly reduced, and there is a risk of problems with workability. Therefore, it is preferable to contain Si within the above range. More preferably, the Si content is 2.0 to 3.9 wt %, and even more preferably, the Si content is 3.0 to 3.5 wt %.
[0018] Al: 0.5~1.5% by weight Aluminum (Al) plays an important role in increasing resistivity together with Si to reduce iron loss, and also plays a role in reducing magnetic anisotropy to reduce magnetic deviation in the rolling direction and the direction perpendicular to the rolling direction. If too little Al is added, fine nitrides are formed or the surface oxide layer is not densely formed, making it difficult to obtain the magnetic improvement effect. If too much Al is added, excessive nitrides are formed, which may deteriorate the magnetic property, causing problems in the process stages such as steelmaking and continuous casting. Therefore, it is preferable to contain Al in the above range. More preferably, Al is contained in an amount of 0.5 to 1.0 wt %.
[0019] Mn:0.05~0.55wt% Manganese (Mn) increases the resistivity of the material, improves core loss, and plays a role in forming sulfides. If too little Mn is added, fine sulfides may be formed, which may cause deterioration of magnetic properties. Conversely, if too much Mn is added, MnS may be excessively precipitated, which may promote the formation of {111} texture, which is unfavorable to magnetic properties, and may cause a rapid decrease in magnetic flux density. More preferably, Mn is contained in an amount of 0.05 to 0.50 wt%.
[0020] C: 0.005% by weight or less Carbon (C) causes magnetic aging and combines with other elements to form carbides, which degrade the magnetic properties, so the lower the C content, the better, and it is best to keep it below 0.005% by weight, and more preferably below 0.003% by weight.
[0021] Ti: 0.004% by weight or less Titanium (Ti) is an element that has a strong tendency to form precipitates in steel, forming fine carbides, nitrides, or sulfides inside the base material, which inhibits grain growth and increases iron loss. Therefore, the Ti content should be controlled to 0.004% by weight or less, and more preferably 0.002% by weight or less.
[0022] N: 0.005% by weight or less Nitrogen (N) not only forms fine AlN precipitates inside the base material, but also combines with other elements to form fine precipitates that inhibit the growth of crystal grains and worsen iron loss, so the lower the N content, the better. Therefore, the N content should be controlled to 0.005% by weight or less, and more preferably 0.003% by weight or less. It is preferable that N satisfies the following formula 1 in relation to Al and Ti. [Formula 1] [N]≦0.005×([Al]+[Ti]) (In formula 1, [N], [Al], and [Ti] represent the contents (wt%) of N, Al, and Ti, respectively.) By controlling the content of Al and Ti, which promote the formation of nitrides, to 0.005 times or less the total content, the formation of fine precipitates can be prevented.
[0023] S: 0.005% by weight or less Sulfur (S) forms fine precipitates, MnS and CuS, which deteriorate the magnetic properties and the hot workability, so it is preferable to control the content to a low level. Therefore, the S content should be controlled to 0.005% by weight or less, more preferably 0.003% by weight or less. It is preferable that S satisfies the following formula 2 in relation to Mn and Cu. [Formula 2] [S]≦0.01×([Mn]+[Cu]) (In formula 2, [S], [Mn] and [Cu] represent the contents (wt%) of S, Mn and Cu, respectively.) By controlling the Mn and Cu contents, which promote the formation of sulfides, to 0.01 times or less the sum of the contents, the formation of fine precipitates can be prevented.
[0024] Cu: 0.01% by weight or less Copper (Cu) forms fine sulfides that deteriorate magnetic properties and reduce hot workability, so its content is preferably controlled low. It is an element that is inevitably present in steel, and it is best to control its content to 0.01 wt% or less. More preferably, Cu is contained at 0.001 to 0.01 wt%.
[0025] One or more of Nb and V may further be included in an amount of up to 0.004 wt % each. Niobium (Nb) and vanadium (V) are elements that have a strong tendency to form precipitates in steel, and they form fine carbides, nitrides, or sulfides inside the base material, inhibiting grain growth and worsening iron loss. Therefore, Nb and V should be controlled to 0.004% by weight or less, and more preferably 0.003% by weight or less, respectively.
[0026] One or more of Cr and Ni may further be included in an amount of 0.05 wt % or less each. Chromium (Cr) and nickel (Ni) do not have a strong tendency to form fine precipitates, but they may form Cr-based carbides that deteriorate the magnetic property or hinder the formation of an Al-based oxide layer in the surface layer, so it is better to control each of them to 0.05% by weight or less, and more preferably to control it to 0.01 to 0.05% by weight.
[0027] One or more of Sn and Sb may further be included in an amount of 0.1 wt % or less each. Tin (Sn) and antimony (Sb) segregate to the surface and grain boundaries of steel and inhibit the development of the initial recrystallization {111} orientation, forming a texture that is favorable for magnetic properties, but since there is a risk of deteriorating workability and surface quality, it is best to keep the content of each below 0.1% by weight, and more preferably, to 0.01 to 0.1% by weight.
[0028] In addition to the elements mentioned above, impurities such as phosphorus (P), boron (B), magnesium (Mg), zirconium (Zr), etc. may be unavoidably mixed in. Although these elements are present in small amounts, they form inclusions in the steel and may cause a deterioration in magnetic properties, so they must be controlled to P: 0.02% or less, B: 0.002% or less, Mg: 0.005% or less, and Zr: 0.005% or less.
[0029] The balance is composed of Fe and inevitable impurities. The inevitable impurities are impurities that are mixed in during the steelmaking stage and the manufacturing process of the grain-oriented electrical steel sheet, and are widely known in the art, so a detailed description will be omitted. In one embodiment of the present invention, the addition of elements other than the above alloy components is not excluded, and various elements may be included within a range that does not harm the technical idea of the present invention. When an additional element is further included, it is included in place of the balance Fe. As described above, in one embodiment of the present invention, the relationship between Al, Mn, Cu, Ti, S, and N is appropriately controlled to form an Al-based oxide layer, thereby improving magnetic properties.
[0030] FIG. 1 shows a schematic cross-sectional view of a non-oriented electrical steel sheet according to one embodiment of the present invention. 1, the non-oriented electrical steel sheet 100 includes an oxide layer 10 extending from the surface toward the inside. The oxide layer 10 contains 50% by weight or more of Al, and the thickness of the oxide layer 10 is 10 to 50 nm. The oxide layer 10 is formed when oxygen in the atmosphere penetrates into the steel sheet during the cooling stage after the final annealing described below. The oxide layer 10 can contain 25% by weight or more of oxygen (O). The oxide layer 10 may contain 50% by weight or more of Al due to surface enrichment of Al. More specifically, the oxide layer 10 may contain 50 to 60% by weight of Al. The remaining alloy components other than Al are the same as the alloy components of the non-oriented electrical steel sheet described above. Since the thickness of the oxide layer 10 is very thin compared to the overall thickness of the non-oriented electrical steel sheet 100, it does not substantially affect the alloy components of the entire grain-oriented electrical steel sheet. Since Al is densely formed in the oxide layer 10 in this manner, the formation of AlN precipitates near the surface layer of the base material is suppressed, which ultimately contributes to improving the magnetic properties.
[0031] Like oxygen, Al also has a concentration gradient in the oxide layer 10. In one embodiment of the present invention, the Al content in the oxide layer 10 means the average Al content in the oxide layer 10. The thickness of the oxide layer 10 is 10 to 50 nm. If the thickness of the oxide layer 10 is too thin, Al concentration may not be performed properly, and the above-mentioned AlN suppression effect may not be sufficiently obtained. If the thickness of the oxide layer 10 is too thick, a large amount of oxygen may penetrate into the steel sheet, resulting in inferior magnetic properties. More preferably, the thickness of the oxide layer 10 is 10 to 30 nm. The oxide layer 10 may have an uneven thickness over the entire surface of the non-oriented electrical steel sheet 100. In one embodiment of the present invention, the thickness of the oxide layer 10 refers to the average thickness over the entire surface of the non-oriented electrical steel sheet 100.
[0032] As described above, the formation of AlN precipitates is suppressed by the presence of the oxide layer 10. Specifically, the number of AlN precipitates with a diameter of 100 nm or less in a cross section from the surface to a depth of 20 μm is 0.1 / mm 2 The diameter and number of AlN precipitates are based on a cross section cut parallel to the thickness direction of the steel sheet, that is, a surface including the thickness direction (ND) of the steel sheet (TD surface, RD surface, etc.). The thickness of the steel plate is 0.1 to 0.3 mm. The average crystal grain size is 50 to 100 μm. When the thickness and average crystal grain size are appropriate, the magnetic properties are improved. The average crystal grain diameter is calculated by [(measurement area ÷ number of crystal grains) 0.5 The calculation is based on a plane parallel to the rolling surface (ND surface).
[0033] As described above, in one embodiment of the present invention, the relationship between Al, Mn, Cu, Ti, S, and N is appropriately controlled to form an Al-based oxide layer, thereby improving magnetic properties. 15 / 50 ) is 1.9W / Kg or less, iron loss (W 10 / 400 ) is 12.5W / kg or less, and the magnetic flux density (B50) is 1.67T or more. 15 / 50 ) is the iron loss when a magnetic flux density of 1.5T is induced at a frequency of 50Hz. Iron loss (W 10 / 400 ) is the iron loss when a magnetic flux density of 1.0T is induced at a frequency of 400Hz. Magnetic flux density (B50) is the magnetic flux density induced in a magnetic field of 5000A / m. More preferably, the iron loss of non-oriented electrical steel sheet (W 15 / 50 ) is 1.9W / Kg or less, iron loss (W 10 / 400 ) is 12.0 W / kg or less, and the magnetic flux density (B50) is 1.68 T or more.
[0034] A method for producing a non-oriented electrical steel sheet according to an embodiment of the present invention includes the steps of hot rolling a slab to produce a hot-rolled sheet, cold rolling the hot-rolled sheet to produce a cold-rolled sheet, final annealing the cold-rolled sheet, and cooling the final-annealed cold-rolled sheet. First, the slab is hot rolled. The alloy composition of the slab has been explained above in connection with the alloy composition of the non-oriented electrical steel sheet, so a duplicate explanation will be omitted. Since the alloy composition does not substantially change during the manufacturing process of the non-oriented electrical steel sheet, the alloy composition of the non-oriented electrical steel sheet and the slab are substantially the same.
[0035] Specifically, the slab consists, by weight, of 1.5-4.0% Si, 0.5-1.5% Al, 0.05-0.55% Mn, 0.005% or less, 0.004% or less (excluding 0%), 0.005% or less (excluding 0%), 0.005% or less (excluding 0%), Cu: 0.01% or less (excluding 0%), with the remainder being Fe and unavoidable impurities, and can satisfy the following formulas 1 and 2. [Formula 1] [N]≦0.005×([Al]+[Ti]) [Formula 2] [S]≦0.01×([Mn]+[Cu]) (In formulas 1 and 2, [N], [Al], [Ti], [S], [Mn] and [Cu] represent the contents (wt%) of N, Al, Ti, S, Mn and Cu, respectively.) Other additional elements have been explained in the alloy components of the non-oriented electrical steel sheet, so duplicate explanations will be omitted.
[0036] The slab may be heated before being hot rolled. There is no restriction on the heating temperature of the slab, but the slab may be heated to 1200°C or less. If the slab heating temperature is excessively high, precipitates such as AlN and MnS present in the slab may be redissolved and then finely precipitated during hot rolling and annealing, suppressing grain growth and decreasing magnetic properties. The slab is hot rolled to produce a hot rolled sheet. The thickness of the hot rolled sheet is 2 to 2.3 mm. At the stage of producing the hot rolled sheet, the finish rolling temperature is 800° C. or higher, preferably 800 to 1000° C. The hot rolled sheet is coiled at a temperature of 700° C. or lower.
[0037] After the step of producing the hot-rolled sheet, the method further includes a step of annealing the hot-rolled sheet. At this time, the annealing temperature of the hot-rolled sheet is 850 to 1150°C. If the annealing temperature of the hot-rolled sheet is too low, the structure does not grow or becomes fine, making it difficult to obtain a texture advantageous for magnetic properties during annealing after cold rolling. If the annealing temperature is too high, the magnetic crystal grains grow excessively, and there is a risk of excessive surface defects on the steel sheet. The hot-rolled sheet annealing is performed to increase the orientation advantageous for magnetic properties as necessary, and can be omitted. The annealed hot-rolled sheet can be pickled. Next, the hot rolled sheet is cold rolled to produce a cold rolled sheet. The cold rolling is final rolling to a thickness of 0.1 mm to 0.3 mm. If necessary, the cold rolling step may include one cold rolling step or two or more cold rolling steps with intermediate annealing in between. In this case, the intermediate annealing temperature is 850 to 1150°C.
[0038] Next, the cold-rolled sheet is subjected to final annealing. There is no limitation on the annealing temperature in the process of annealing the cold-rolled sheet, so long as it is a temperature normally used for non-oriented electrical steel sheets. Since the core loss of non-oriented electrical steel sheets is closely related to the grain size, a temperature of 700 to 1050°C is preferable, and the average grain size can be 50 to 100 μm during the final annealing process, and all (99% or more) of the processed structure formed in the previous cold rolling stage is recrystallized.
[0039] The final annealing step can be performed for 50 to 90 seconds in a non-oxidizing atmosphere, which contains 5% by volume or more of H2 and has a dew point of 0°C or lower. Next, the final annealed cold-rolled sheet is cooled. After the cold-rolled sheet is finally cooled to below 100°C, an insulating coating can be formed. During the final annealing process, oxygen in the atmosphere penetrates the steel sheet while the steel sheet is cooled to below 700°C, forming an oxide layer 10. At this time, the thickness of the oxide layer 10 can be adjusted by adjusting the time of exposure to the oxygen-containing atmosphere. At temperatures below 300°C, oxygen is difficult to penetrate the steel sheet, and the exposure time at this time does not affect the thickness of the oxide layer 10.
[0040] The exposure time is 5 to 20 seconds. If the exposure time is too short, the oxide layer 10 is formed thinly, and if the exposure time is too long, the oxide layer 10 is formed thickly. More specifically, the exposure time is preferably 10 to 17 seconds. The atmosphere is an oxidizing atmosphere with a dew point above 0°C. The present invention will be described in more detail with reference to the following examples, which are merely for illustrative purposes and are not intended to limit the scope of the present invention.
[0041] Working Example Steel ingots containing the materials shown in Tables 1 and 2 and the balance Fe and unavoidable impurities were produced by vacuum melting in a laboratory. These were reheated at 1150°C and hot rolled at a finishing temperature of 880°C to produce hot rolled sheets with a thickness of 2.0 mm. The hot rolled sheets were annealed at 1030°C for 100 seconds and then cold rolled to produce the thicknesses shown in Table 3. These were then subjected to final recrystallization annealing at 1000°C for about 80 seconds in an atmosphere of 80% N2 by volume and 20% H2 by volume. Thereafter, when cooling from 700°C to 300°C, the time of exposure to an atmosphere with a dew point above 0°C was adjusted as shown in Table 3 below. The crystal grain size, the thickness of the oxide layer, the Al content of the oxide layer, and the distribution of AlN particles with diameters of 100 nm or less at a depth of 20 μm from the surface for each specimen are shown in Table 3 below. The grain size was measured by polishing and etching the cross section of the test piece perpendicular to the rolling direction, and photographing an area sufficient to include at least 1,500 grains with an optical microscope, and then dividing the measured area by the number of grains by the measured area. 0.5 ] was calculated using the formula:
[0042] The magnetic properties such as magnetic flux density and core loss were measured by cutting 5 pieces of 60mm wide x 60mm long for each specimen and measuring them in the rolling direction and perpendicular direction with a single sheet tester. The average values were calculated. 10 / 400 is the core loss when a magnetic flux density of 1.0 T is induced at a frequency of 400 Hz, and B50 means the magnetic flux density induced in a magnetic field of 5000 A / m. The oxide layer thickness was determined by processing the specimen with FIB to create a smooth cross section, photographing it with a high-resolution TEM, and calculating the average thickness of the oxide layer at more than 10 points. The aluminum content of the oxide layer refers to the aluminum content expressed in weight percent when the components of the oxide layer were measured using the TEM-EDS method. AlN less than 100nm indicates the number of AlN precipitates with a diameter of 100nm or less that exist in the region from the surface to a depth of 20μm when the precipitates were observed with a TEM.
[0043] [Table 1]
[0044] [Table 2]
[0045] [Table 3]
[0046] As shown in Tables 1 to 3, in the cases of A3, A4, B3, B4, C3, C4, D3, D4, E3, and E4, the component contents and manufacturing methods all satisfy the specific ranges of the present invention, and the crystal grain size, thickness and Al content of the oxide layer, and AlN distribution in the surface layer of 100 nm or less are well formed, and it can be confirmed that the magnetism at high frequencies is excellent. On the other hand, in the cases of A1, A2, B2, and C2, the contents of N, S, Ti, and Cu exceeded the range of the present invention, and excessive AlN of 100 nm or less was formed in the surface layer, making it impossible to ensure excellent high-frequency magnetism. In the cases of B1 and C1, the exposure time to the oxidizing atmosphere was long or short, resulting in the formation of a thick or thin oxide layer, which was confirmed to result in relatively poor high frequency magnetism.
[0047] C2 was cooled after annealing in a non-oxidizing atmosphere of 15% H2 with a dew point of -20°C to 300°C. As a result, no oxide layer was formed, and it was confirmed that the high frequency magnetism was relatively inferior. In D1, D2, E1, and E2, the Al and Mn contents did not reach or exceeded the range of the present invention, resulting in the formation of fine AlN in the surface layer or an excessively thick oxide layer in the surface layer, which deteriorated the magnetic properties at high frequencies.
[0048] The present invention is not limited to the above-described embodiment, but can be manufactured in various different forms, and a person having ordinary skill in the art to which the present invention pertains should understand that the present invention can be embodied in other specific forms without changing the technical concept or essential features of the present invention. Therefore, it should be understood that the above-described embodiment is illustrative in all respects and is not limiting. [Explanation of symbols]
[0049] 100: Non-oriented electrical steel sheet 10: Oxide layer
Claims
1. In weight percent, Si: 1.5 to 4.0%, Al: 0.5 to 1.5%, Mn: 0.05 to 0.55%, C: 0.005% or less, Ti: 0.004% or less (excluding 0%), N: 0.005% or less (excluding 0%), S: 0.005% or less (excluding 0%), Cu: 0.01% or less (excluding 0%), with the balance being Fe and unavoidable impurities, The following formulas 1 and 2 are satisfied: The steel sheet includes an oxide layer extending from the outermost surface to the inside, The oxide layer contains 50% by weight or more of Al, the thickness of the oxide layer is 10 to 50 nm; The number of AlN precipitates with a diameter of 100 nm or less in a cross section from the outermost surface to a depth of 20 μm of the steel plate is 0.1 / mm 2 A non-oriented electrical steel sheet characterized in that: [Formula 1] [N]≦0.005×([Al]+[Ti]) [Formula 2] [S]≦0.01×([Mn]+[Cu]) (In Formula 1 and Formula 2, [N], [Al], [Ti], [S], [Mn] and [Cu] represent the contents (wt%) of N, Al, Ti, S, Mn and Cu, respectively.)
2. 2. The non-oriented electrical steel sheet according to claim 1, further comprising at least one of Nb and V in an amount of 0.004% by weight or less.
3. 3. The non-oriented electrical steel sheet according to claim 1, further comprising 0.05% by weight or less of one or more of Cr and Ni.
4. The non-oriented electrical steel sheet according to claim 1 , further comprising at least one of Sn and Sb in an amount of 0.1% by weight or less each.
5. 5. The non-oriented electrical steel sheet according to claim 1, further comprising one or more of P: 0.02 wt % or less, B: 0.002 wt % or less, Mg: 0.005 wt % or less, and Zr: 0.005 wt % or less.
6. The non-oriented electrical steel sheet according to any one of claims 1 to 5, characterized in that the average crystal grain size is 50 to 100 µm.
7. A method for producing a non-oriented electrical steel sheet according to any one of claims 1 to 6, comprising the steps of: a step of producing a hot-rolled sheet by hot rolling a slab which contains, in weight percent, 1.5 to 4.0% Si, 0.5 to 1.5% Al, 0.05 to 0.55% Mn, 0.005% or less C, 0.004% or less (except 0%) Ti, 0.005% or less (except 0%) N, 0.005% or less (except 0%) S, 0.005% or less (except 0%) Cu, the balance being Fe and unavoidable impurities, and which satisfies the following formulas 1 and 2; cold rolling the hot rolled sheet to produce a cold rolled sheet; final annealing the cold rolled sheet; and Cooling the final annealed cold rolled sheet, In the step of cooling the final annealed cold-rolled sheet, the time for exposing the sheet to an atmosphere having a dew point exceeding 0° C. at a temperature of 700° C. or less for 5 to 20 seconds. [Formula 1] [N]≦0.005×([Al]+[Ti]) [Formula 2] [S]≦0.01×([Mn]+[Cu]) (In Formula 1 and Formula 2, [N], [Al], [Ti], [S], [Mn] and [Cu] represent the contents (wt%) of N, Al, Ti, S, Mn and Cu, respectively.)
8. The method for producing a non-oriented electrical steel sheet according to claim 7, further comprising the step of heating the slab at a temperature of 1200° C. or less before the step of producing the hot rolled sheet.
9. The method of claim 7, wherein the hot rolling step has a finish rolling temperature of 800° C. or more.
10. The method for producing a non-oriented electrical steel sheet according to any one of claims 7 to 9, further comprising the step of annealing the hot-rolled sheet at a temperature in the range of 850 to 1150°C after the hot-rolling step.
11. The method for manufacturing a non-oriented electrical steel sheet according to any one of claims 7 to 10, wherein the final annealing step comprises annealing in a non-oxidizing atmosphere at a temperature of 700 to 1050°C for 50 to 90 seconds.
12. The non-oxidizing atmosphere is H 2 and a dew point of 0° C. or lower.
Citation Information
Patent Citations
Non-oriented magnetic steel sheet having good entire circumferential magnetic property
JP2016003371A
Non-oriented electrical steel sheet and its manufacturing method
JP2019507243A
Non-oriented electromagnetic steel sheet with low iron loss and adequate workability, and manufacturing method therefor
KR1020100037705A
Non-oriented electrical steel sheet and method for manufacturing the same
KR1020190078251A
Non-oriented electromagnetic steel sheet and process for production thereof
WO2011102328A1