980MPa level all-bainite type ultra-high hole expandability steel and its manufacturing method

The 980 MPa all-bainitic ultra-high hole expandability steel achieves a balance of high strength and hole expansion rate through a specific chemical composition and controlled manufacturing process, resulting in a homogeneous bainite structure for improved performance in automobile chassis parts.

JP7594662B2Active Publication Date: 2024-12-04BAOSHAN IRON & STEEL CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023513796
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-08-31
Filing Date
2021-08-30
Publication Date
2024-12-04
Estimated Expiration
2041-08-30

AI Technical Summary

Technical Problem

Existing high-strength steels face challenges in achieving a balance between high elongation and high hole expansion rate, particularly at the 980 MPa level, with most literature focusing on lower strength levels and lacking inhomogeneous structures adversely affecting performance.

Method used

A chemical composition of 980 MPa level all-bainitic ultra-high hole expandability steel with specific elements like C, Si, Mn, P, S, Al, N, Mo, Ti, Cr, B, Ca, Nb, V, Cu, and Ni, combined with a manufacturing process involving smelting, hot rolling, and controlled cooling to achieve a homogeneous, single-phase bainite structure.

Benefits of technology

The solution results in a steel with yield strength ≥800 MPa, tensile strength ≥980 MPa, and hole expansion rate ≥60%, exhibiting excellent strength, plasticity, toughness, and cold bending performance, suitable for complex automobile chassis parts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007594662000005
    Figure 0007594662000005
  • Figure 0007594662000006
    Figure 0007594662000006
  • Figure 0007594662000007
    Figure 0007594662000007
Patent Text Reader

Abstract

An all-bainite ultra-high hole-expandability steel with a strength of 980 MPa, having a chemical composition, by weight percentage, of 0.05-0.10% C, 2.0% Si or less, 1.0-2.0% Mn, 0.02% P or less, 0.003% S or less, 0.02-0.08% Al, 0.004% N or less, 0.1-0.5% Mo, 0.01-0.05% Ti, and 0.0030% O or less, with the balance being Fe and other unavoidable impurities, and a method for producing the same. The ultra-high hole-expandability steel of the present invention has a yield strength of 800 MPa or more, a tensile strength of 980 MPa or more, and a hole expansion ratio of 60% or more, making it suitable for use in passenger vehicle chassis parts that require high strength and thin wall thickness and require complex forming, such as control arms and subframes.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention belongs to the field of high strength steel, and in particular relates to a full bainite type ultra-high hole expandability steel having a strength of 980 MPa and a method for producing the same. [Background technology]

[0002] With the development of the national economy, the number of automobiles produced has increased significantly, and the amount of plate materials used has also continued to increase. In China's domestic automobile industry, the original design of many vehicle model parts, such as automobile chassis parts, torsion beams, sedan subframes, wheel spokes and rims, front and rear axle assemblies, body structural parts, seats, clutches, seat belts, truck box panels, protective nets, car beams, etc., requires the use of hot-rolled plates and pickled plates. Among them, chassis steel accounts for 24-34% of the total amount of steel used in automobiles.

[0003] Lightweighting of passenger cars is not only a trend in the automotive industry, but also a requirement of regulations. Regulations stipulate fuel efficiency, but this is essentially a requirement for lighter body construction, which translates into higher strength, thinner walls, and lighter materials. Higher strength and lighter weight are inevitable requirements for future new car models, which will inevitably lead to higher steel usage levels and changes in chassis structure: for example, the increasing complexity of parts will lead to higher requirements for material performance and surface, as well as advances in forming technologies such as hydroforming, hot stamping, and laser welding, which will result in higher material strength, stamping, flanging, rebound, fatigue, and other performance.

[0004] Compared with overseas, the development of high-strength high-hole-expandability steel in China not only has a relatively low strength level, but also has poor performance stability. For example, most of the high-hole-expandability steels used by domestic auto parts manufacturers in China are high-hardness steels with a strength of 600 MPa or less, and the competition for high-hole-expandability steels with a strength of 440 MPa or less is intensifying. At present, high-hole-expandability steels with a tensile strength of 780 MPa are gradually being mass-produced, but the requirements for elongation and hole expansion ratio, which are two important indicators of forming, will also be higher. On the other hand, high-hole-expandability steels with a strength of 980 MPa are still in the research and development and certification stage and have not yet reached the stage of mass production. However, 980 high-hole-expandability steels with higher strength and ultra-high hole expansion ratio will inevitably be the direction of future development. In order to meet the potential needs of users, there is a demand for the development of high-hole-expandability steels with excellent hole expansion properties at the 980 MPa level.

[0005] Most of the existing patent documents are related to high hole expandability steels at 780 MPa or less. There are few documents related to high hole expandability steels at 980 MPa. Chinese patent application CN106119702A discloses a hot-rolled high hole expandability steel at 980 MPa, which has a fine structure of granular bainite and a small amount of martensite, and the main feature of its composition design is a low-carbon V-Ti fine alloying design with trace amounts of Nb and Cr added. It is significantly different from the present invention in terms of composition, process, structure, etc. Summary of the Invention [Problem to be solved by the invention]

[0006] According to the literature, the elongation of a material is usually inversely proportional to its hole expansion ratio, i.e., the higher the elongation, the lower the hole expansion ratio, and conversely, the lower the elongation, the higher the hole expansion ratio. It is therefore very difficult to obtain a high hole-expandability steel that has high elongation and high hole expandability and at the same time high strength. Also, with the same or similar strengthening mechanism, the higher the strength of the material, the lower the hole expansion ratio.

[0007] To obtain steel materials with excellent plasticity and hole expansion / flanging properties, it is necessary to strike a better balance between the two. Of course, the hole expansion ratio of a material is closely related to many factors, among which the homogeneity of the structure, the control level of inclusions and segregation, the type of structure, and the measurement of the hole expansion ratio are the most important factors. In general, a single and homogeneous structure is favorable for improving the hole expansion ratio, while a two-phase or multi-phase structure is unfavorable for improving the hole expansion ratio. [Means for solving the problem]

[0008] Contents of the invention An object of the present invention is to provide a fully bainite type ultra-high hole expandability steel with a strength of 980 MPa and a manufacturing method thereof, and the ultra-high hole expandability steel has a yield strength of 800 MPa or more, a tensile strength of 980 MPa or more, and a hole expansion ratio of 60% or more, and can be used for passenger vehicle chassis parts that require high strength and thin wall thickness and are complex to form, such as control arms and subframes.

[0009] To achieve the above objectives, the technical solution of the present invention: According to the composition design of the present invention, the C content is designed to be low in order to ensure excellent weldability during use by the user and to ensure compatibility between the excellent strength and hole expansion ratio of the obtained bainite structure.

[0010] Specifically, the chemical composition of the all-bainite type ultra-high hole expandability steel of the present invention having a strength of 980 MPa is, in weight percentages, 0.05 to 0.10% C, ≦2.0% Si, 1.0 to 2.0% Mn, ≦0.02%, ≦0.003%, 0.02 to 0.08%, ≦0.004%, 0.1 to 0.5% Mo, 0.01 to 0.05% Ti, with the balance being Fe and other unavoidable impurities.

[0011] The steel further contains one or more elements selected from the group consisting of Cr≦0.5%, B≦0.002%, Ca≦0.005%, Nb≦0.06%, V≦0.05%, Cu≦0.5%, and Ni≦0.5%; however, the preferred contents of Nb and V are each ≦0.03%. In some embodiments, the all-bainite type ultra-high hole expandability steel of 980 MPa level according to the present invention contains Cr and / or B, the preferred content of Cr is 0.20-0.50%, and the preferred content of B is 0.0005-0.002%. The preferred contents of Cu and Ni are each ≦0.3%, the preferred content of Cr is 0.2-0.4%, the preferred content of B is 0.0005-0.0015%, and the preferred content of Ca is ≦0.002%.

[0012] In some embodiments, the all-bainite type ultra-high hole expandability steel of the present invention has a chemical composition, in weight percentages, of C 0.05 to 0.10%, Si≦2.0%, Mn 1.0 to 2.0%, P≦0.02%, S≦0.003%, Al 0.02 to 0.08%, N≦0.004%, Mo 0.1 to 0.5%, Ti 0.01 to 0.05%, Cr≦0.5%, B≦0.002%, Ca≦0.005%, Nb≦0.06%, V≦0.05%, Cu≦0.5%, Ni≦0.5%, and the balance is Fe and other unavoidable impurities. The all-bainite type ultra-high hole expandability steel contains at least one or more elements selected from Cr, B, Ca, Nb, V, Cu, and Ni, and preferably contains at least Cr and / or B.

[0013] Preferably, the C content is 0.06-0.09%. Preferably, the Mn content is 1.4-1.8%. Preferably, the S content is controlled to 0.0015% or less. Preferably, the Al content is 0.02-0.05%. Preferably, the N content is controlled to 0.003% or less. Preferably, the Ti content is 0.01-0.03%. Preferably, the Mo content is 0.15-0.35%. Preferably, the O content is controlled to within 30 ppm. Preferably, the Si content is 0.05-2.0%.

[0014] The microstructure of the ultra-high hole expandability steel according to the present invention is entirely bainite. The ultra-high hole expandability steel according to the present invention has a yield strength of ≧800 MPa, preferably ≧830 MPa, more preferably ≧850 MPa, and even more preferably ≧880 MPa, a tensile strength of ≧980 MPa, preferably ≧1000 MPa, and more preferably ≧1020 MPa, and a lateral elongation A 50 ≧10%, hole expansion ratio ≧60%, preferably ≧70%, and passes the cold bending performance test (d≦4a, 180°).

[0015] Preferably, the ultra-high hole-expandability steel according to the present invention has a −40° C. impact toughness of ≧40 J, preferably ≧50 J, more preferably ≧60 J. In a particularly preferred embodiment, the ultra-high hole-expandability steel according to the present invention has a −40° C. impact toughness of ≧70 J.

[0016] In a preferred embodiment, the ultra-high hole-expandability steel according to the present invention has a yield strength of ≥ 850 MPa, a tensile strength of ≥ 1020 MPa, and a lateral elongation A 50 ≧10%, hole expansion ratio ≧70%, -40℃ impact toughness ≧50J, and passed the cold bending performance test (d≦4a, 180°).

[0017] In a further preferred embodiment, the ultra-high hole-expandability steel according to the present invention has a yield strength of ≥ 830 MPa, a tensile strength of ≥ 1000 MPa, and a lateral elongation A 50 ≧10%, hole expansion ratio ≧70%, -40℃ impact toughness ≧60J, and passed the cold bending performance test (d≦4a, 180°).

[0018] In a further preferred embodiment, the ultra-high hole-expandability steel according to the present invention has a yield strength of ≥ 900 MPa, a tensile strength of ≥ 1040 MPa, and a lateral elongation A 50 ≧10%, hole expansion ratio ≧65%, -40℃ impact toughness ≧40J, and passed the cold bending performance test (d≦4a, 180°).

[0019] In the composition design of the ultra-high hole expandability steel according to the present invention: Carbon is a basic element in steel and is also one of the important elements for the present invention. Carbon expands the austenite phase region and stabilizes austenite. Carbon, as an interstitial atom in steel, plays a very important role in improving the strength of steel, and has the greatest effect on the yield strength and tensile strength of steel. In the present invention, in order to obtain ultra-high strength and ultra-high hole expansion ratio, it is necessary to obtain a single-phase homogeneous low-carbon bainite structure. In order to obtain high-strength steel with a tensile strength of 980 MPa, it is necessary to ensure that the carbon content is 0.05% or more, otherwise, if the carbon content is 0.05% or less, the tensile strength of the bainite structure formed cannot reach 980 MPa. However, the carbon content must not exceed 0.10%. If the carbon content is too high, many island martensite-austenite constituents are likely to occur in the low-carbon bainite structure formed, which is disadvantageous to elongation and hole expansion ratio. Therefore, the carbon content should be controlled between 0.05 and 0.10%, with the preferred range being between 0.06 and 0.09%.

[0020] Silicon is a basic element in steel and is also one of the important elements for the present invention. As mentioned above, different silicon contents have an important effect on the performance of steel, especially on elongation and hole expansion ratio. When the silicon content is low, the amount of retained austenite in the structure is small, and the elongation is relatively low. However, when the silicon content reaches 0.8% or more, the content of retained austenite in the structure increases in the same process, which is favorable for improving elongation. Within the silicon content range of the present invention, different silicon contents mainly affect the elongation index, but have little effect on the hole expansion ratio. Adding a lot of silicon to steel is likely to increase the load of the rolling machine, which is also disadvantageous to the surface of the steel. Therefore, in order to improve the surface quality of the steel and reduce the actual rolling force, the Si content in the steel cannot be allowed to be too high, and usually does not exceed 2.0%. According to the actual needs of users, two concepts of low silicon and high silicon can be adopted in the component design, respectively.

[0021] Manganese is the most basic element in steel and is one of the most important elements for the present invention. As is well known, Mn is an important element that expands the austenite phase region, reduces the critical quenching rate of steel, stabilizes austenite, refines crystal grains, and delays the transformation from austenite to pearlite. In the present invention, in order to ensure the strength of the steel plate, the Mn content is usually controlled to 1.0% or more, but the Mn content is usually not allowed to exceed 2.0%, otherwise, segregation of Mn is likely to occur during steelmaking, and hot cracks are likely to occur during continuous slab casting. Therefore, in steel, the Mn content is usually controlled to 1.0-2.0%, with a preferred range of 1.4-1.8%.

[0022] Phosphorus is an impurity element in steel. P tends to be concentrated in grain boundaries, and if the P content in steel is high (≧0.1%), it forms Fe2P and precipitates around grains, reducing the plasticity and toughness of the steel. Therefore, the lower the P content, the better. In general, it is preferable to control it to within 0.02%, and the steelmaking cost will not increase.

[0023] Sulfur is an impurity element in steel. S in steel usually combines with Mn to form MnS inclusions. Especially when the contents of S and Mn are both high, a lot of MnS is formed in the steel. MnS itself has some plasticity, and in the subsequent rolling process, MnS deforms along the rolling direction, which not only reduces the transverse plasticity of the steel sheet, but also increases the anisotropy of the structure, which is disadvantageous to the hole expandability. Therefore, the lower the S content in steel, the better. Considering that the Mn content in the present invention must be at a high level, the S content must be strictly controlled in order to reduce the MnS content. The S content must be controlled within 0.003%, and the preferred range is 0.0015% or less.

[0024] In steel, aluminum mainly plays the role of deoxidization and nitrogen fixation. Assuming the presence of strong carbide forming elements such as Ti, Nb, and V, Al mainly plays the role of deoxidization and grain refinement. In the present invention, Al is a general deoxidizing element and grain refinement element, and its content may be controlled to usually 0.02 to 0.08%. If the Al content is less than 0.02%, it cannot contribute to grain refinement, and similarly, if the Al content is 0.08% or more, its grain refinement effect is saturated. Therefore, in steel, the Al content may be controlled usually between 0.02 and 0.08%, with the preferred range being between 0.02 and 0.05%.

[0025] In the present invention, nitrogen belongs to the impurity element, and the lower its content, the better. However, nitrogen is an unavoidable element in the steelmaking process. Although its content is small, when it is combined with strong carbide forming elements such as Ti, the formed TiN particles have a very negative effect on the performance of the steel, especially the hole expandability. In addition, since TiN has a square shape, there is a large stress concentration between its sharp corners and the substrate, and during the hole expansion deformation process, cracks are likely to occur due to the stress concentration between TiN and the substrate, which greatly reduces the hole expandability. On the premise that the nitrogen content is controlled as much as possible, the lower the content of strong carbide forming elements such as Ti, the better. In the present invention, the adverse effects of TiN are reduced as much as possible by adding a trace amount of Ti to fix nitrogen. Therefore, the nitrogen content should be controlled to 0.004% or less, and the preferred range is 0.003% or less.

[0026] Titanium is one of the important elements for the present invention. Ti plays two main roles in the present invention: one is to combine with the impurity element N in the steel to form TiN, which plays a part of the role of "nitrogen fixation"; the other is to form a certain number of fine TiN dispersed in the subsequent welding process of the material, suppress the size of austenite crystal grains, refine the structure, and improve low-temperature toughness. Therefore, in steel, the Ti content range is controlled to 0.01-0.05%, and the preferred range is 0.01-0.03%.

[0027] Molybdenum is one of the important elements for the present invention. Adding molybdenum to steel can significantly delay the transformation of ferrite and pearlite. This role of molybdenum is advantageous for adjusting various processes in the actual rolling process. For example, at the end of rolling, stepwise cooling may be performed, or air cooling followed by water cooling may be performed. In the present invention, even if the process of air cooling followed by water cooling or the process of direct water cooling after rolling is adopted, the addition of molybdenum can ensure that structures such as ferrite and pearlite are not formed during the air cooling process, and dynamic recovery of austenite deformed during the air cooling process occurs, contributing to the improvement of the homogeneity of the structure; molybdenum has strong resistance to welding softening. The main purpose of the present invention is to obtain a structure of a single low-carbon martensite and a small amount of retained austenite, but since low-carbon martensite is prone to softening phenomenon after welding, the degree of welding softening can be effectively reduced by adding a certain amount of molybdenum. Therefore, the molybdenum content should be controlled between 0.1 and 0.5%, with the preferred range being 0.15 to 0.35%.

[0028] Chromium is one of the elements that can be added in the present invention. The addition of a small amount of chromium is not for improving the hardenability of steel, but for combining with the B phase to contribute to the formation of an acicular ferrite structure in the weld heat affected zone after welding, thereby significantly improving the low-temperature toughness of the weld heat affected zone. Since the final application part according to the present invention is a chassis product for passenger cars, the low-temperature toughness of the weld heat affected zone is an important indicator. In addition to ensuring that the strength of the weld heat affected zone does not decrease too much, the low-temperature toughness of the weld heat affected zone must also meet certain requirements. In addition, chromium itself has a certain degree of weld softening resistance. Therefore, in steel, the amount of chromium added is usually ≦0.5%, and the preferred range is 0.2-0.4%.

[0029] Boron is one of the elements that can be added in the present invention. The main role of boron in steel is to be unevenly distributed in the prior austenite grain boundaries and to suppress the formation of proeutectoid ferrite; adding boron to steel can also greatly improve the hardenability of the steel. However, in the present invention, the main purpose of adding a trace amount of boron is not to improve the hardenability, but to combine with the chromium phase to improve the structure of the weld heat affected zone and obtain an acicular ferrite structure with excellent toughness. The boron element added to steel is usually controlled to 0.002% or less, and the preferred range is between 0.0005 and 0.0015%.

[0030] Calcium is an element that can be added to the present invention. Calcium improves the morphology of sulfides such as MnS, converts long-striped sulfides such as MnS into spherical CaS, and contributes to improving the morphology of inclusions, thereby reducing the adverse effect of long-striped sulfides on hole expandability. However, if too much calcium is added, the number of calcium oxides increases, which is detrimental to hole expandability. Therefore, in steel, the amount of calcium added is usually ≦0.005%, and the preferred range is ≦0.002%.

[0031] Oxygen is an inevitable element in the steelmaking process, and in the present invention, the O content in steel can usually reach 30 ppm or less after deoxidation, and there is no obvious adverse effect on the performance of the steel sheet. Therefore, it is sufficient to control the O content in steel to within 30 ppm.

[0032] Niobium is one of the elements that can be added in the present invention. Niobium, like titanium, is a strong carbide-forming element in steel. By adding niobium to steel, the non-recrystallization temperature of steel can be significantly increased, and deformed austenite with higher dislocation density can be obtained in the finish rolling stage, and the final transformation structure can be refined in the subsequent transformation process. However, the amount of niobium added should not be too much. On the other hand, if the amount of niobium added exceeds 0.06%, it is easy to form relatively coarse niobium carbonitride in the structure, consuming part of the carbon atoms and reducing the precipitation strengthening effect of carbides. In addition, if the niobium content is high, anisotropy is easily generated in the austenite structure in the hot rolled state, which is carried over to the final structure in the subsequent cooling transformation process, which is disadvantageous to hole expansion properties. Therefore, in steel, the niobium content is usually controlled to ≦0.06%, and the preferred range is ≦0.03%.

[0033] Vanadium is an element that can be added in the present invention. Vanadium, like titanium and niobium, is a strong carbide-forming element. However, vanadium carbides have low solid solution and precipitation temperatures, and are usually all dissolved in austenite at the finish rolling stage. Only when the temperature drops and transformation begins does vanadium begin to form in ferrite. The solid solubility of vanadium carbides in ferrite is greater than that of niobium and titanium, so vanadium carbides are formed in larger sizes in ferrite, which is unfavorable to precipitation strengthening, and their contribution to the strength of steel is much smaller than that of titanium, and the formation of vanadium carbides consumes carbon atoms to a certain extent, which is unfavorable to improving the strength of steel. Therefore, in steel, the vanadium addition amount is usually ≦0.05%, and the preferred range is ≦0.03%.

[0034] Copper is one of the elements that can be added in the present invention. The addition of copper to steel can improve the corrosion resistance of the steel, and when added together with P, the corrosion resistance is even better; when the amount of Cu added exceeds 1%, it can form an ε-Cu precipitate phase under certain conditions, and can achieve a strong precipitation strengthening effect. However, the addition of Cu is likely to cause the "Cu embrittlement" phenomenon during the rolling process, and in order to fully utilize the corrosion resistance improvement effect of Cu without significantly causing the "Cu embrittlement" phenomenon in a certain application environment, the Cu element content is usually controlled within 0.5%, with the preferred range being within 0.3%.

[0035] Nickel is one of the elements that can be added in the present invention. The addition of nickel to steel gives it a certain degree of corrosion resistance, but the corrosion resistance effect is weaker than that of copper. The addition of nickel to steel does not affect the tensile performance of the steel very much, but it can refine the structure and precipitation phase of the steel and greatly improve the low-temperature toughness of the steel; in addition, the addition of a small amount of nickel to steel with the addition of copper element can suppress the occurrence of "Cu embrittlement". The addition of a large amount of nickel has no obvious adverse effect on the performance of the steel itself. The simultaneous addition of copper and nickel not only improves the corrosion resistance, but also refines the structure and precipitation phase of the steel, and greatly improves the low-temperature toughness. However, since both copper and nickel are relatively expensive alloying elements, in order to minimize the cost of alloy design, the amount of nickel added is usually ≦0.5%, and the preferred range is ≦0.3%.

[0036] The manufacturing method of the present invention for producing a full bainite type ultra-high hole expandability steel with a strength of 980 MPa includes the following steps: 1) Smelting and casting Smelting in a converter or electric furnace according to the composition described, followed by secondary refining in a vacuum furnace, then casting into billets or ingots; 2) Reheat the billet or ingot at a heating temperature of 1100 to 1200°C and a heat retention time of 1 to 2 hours; 3) Hot rolling For the main purpose of refining austenite grains, the rolling start temperature is 950-1100°C, 3-5 passes are performed under high pressure at 950°C or higher, and the cumulative deformation amount is ≧50%, preferably ≧70%; next, the intermediate billet temperature is 930-950°C, and then 5-7 passes of finish rolling are performed, and the cumulative deformation amount is ≧70%, preferably ≧80%; the rolling end temperature is 800-930°C; 4) Cooling First, air-cool for 0 to 10 seconds to allow dynamic recovery and dynamic recrystallization, then water-cool, and then heat the material to the bainite transformation temperature range, i.e., B s ~B f The steel strip is water-cooled at a cooling rate of ≧10°C / s, preferably 10-60°C / s, and then coiled, and the steel coil is cooled to room temperature by air cooling (cooling rate >20°C / h); the preferred coiling temperature is 410-550°C; 5) Pickling The pickling speed of the steel strip is adjusted in the range of 30-100 m / min, the pickling temperature is controlled between 75-85°C, and the tensile straightening rate is controlled to be ≦2% so as to reduce the elongation loss of the steel strip; the steel strip is rinsed in the temperature range of 35-50°C, and the surface of the steel strip is dried and oiled at 120-140°C.

[0037] Preferably, after pickling in step 5), rinsing is performed in the temperature range of 35 to 50°C, and the surface of the steel strip is dried at a temperature of 120 to 140°C and oiled.

[0038] The innovations of the present invention are as follows: According to the composition design of the present invention, a design concept of single-phase low-carbon bainite is adopted, a suitable rolling end temperature and air cooling or direct water cooling after rolling are adopted, and air cooling or other modes that can accelerate the cooling of the steel coil are adopted for the wound steel coil, so that the temperature of the steel coil is cooled to room temperature as quickly as possible, thereby finally obtaining a single-phase bainite with a homogeneous structure and fine structure, which exhibits high plasticity, toughness, good cold bending performance and ultra-high hole expansion ratio.

[0039] In the design of the rolling process, the rolling process should be completed as fast as possible in the rough rolling and finish rolling stages. After the rolling is completed, air cooling should be performed at different times, but laminar cooling can also be performed directly after the rolling is completed. The main purpose of air cooling is to design the composition with a large amount of manganese and molybdenum, where manganese is an element that stabilizes austenite, and molybdenum significantly delays the ferrite and pearlite transformation. Therefore, in the process of air cooling for a certain time, the rolled deformed austenite undergoes dynamic recrystallization and relaxation without transformation, that is, without forming a ferrite structure. When the deformed austenite undergoes dynamic recrystallization, it can form austenite with a homogeneous structure and pseudo-equixized structure, and after relaxation, the dislocations inside the austenite grains are greatly reduced. The combination of the two can obtain a single-phase bainite with a homogeneous structure and fine structure in the subsequent water-cooled laminar cooling process. In order to obtain a bainite structure, the water cooling rate of the strip steel should be ≧10℃ / s.

[0040] Since the microstructure according to the present invention is low carbon bainite, the bainite transformation temperature range, i.e., B s ~B f The steel strip can be cooled and coiled at a cooling rate of ≧10° C. / s during the cooling period. Because the bainite transformation time is long, the transformation occurs even after the steel coil is coiled. Therefore, in order to obtain high-strength steel with excellent strength, plasticity, and hole expansion ratio, it is necessary to obtain a single-phase homogeneous and fine bainite structure by cooling the coiled steel coil to room temperature as quickly as possible in the shortest time using air cooling or other forced cooling modes (cooling rate >20° C. / h, preferably ≧25° C. / h). Based on such innovative components and process design concepts, the present invention can obtain a 980 MPa level all-bainite type ultra-high hole expandability steel with excellent performance in terms of strength, plasticity, toughness, cold bending, hole expandability, etc.

[0041] The advantageous effects of the present invention are: (1)By adopting a relatively economical composition design concept and an innovative cooling process route, we have obtained a 980MPa level ultra-high hole expandability steel with excellent properties such as strength, plasticity, toughness, and hole expandability; (2) The steel coil or steel plate has excellent strength, plasticity, toughness and hole expansion ratio compatibility, and also has good cold bending performance and hole expansion / flanging performance. Its yield strength is ≧800MPa, tensile strength is ≧980MPa, and it is a hot-rolled or pickled ultra-high hole expansion steel with a thickness of 2-6mm, and has good elongation (transverse A 50 It also has excellent impact toughness and hole expandability (hole expansion ratio ≧ 8%), and can be used in the manufacture of automobile chassis and subframes and other parts that require high strength, thinning, hole expansion and flanging, and are complex to mold, and is expected to have a very wide range of applications. [Brief description of the drawings]

[0042] [Figure 1] FIG. 1 is a process flow chart of a method for producing a full bainite type ultra-high hole expandability steel of 980 MPa level according to the present invention. [Diagram 2] FIG. 2 is a conceptual diagram of a rolling process in a manufacturing method of a full bainite type ultra-high hole expandability steel of 980 MPa level according to the present invention. [Diagram 3] FIG. 3 is a conceptual diagram of a cooling process in a manufacturing method of a full bainite type ultra-high hole expandability steel of 980 MPa level according to the present invention. [Figure 4] FIG. 4 is a typical metal structure photograph of Example 3 of the ultra-high hole expandability steel according to the present invention. [Diagram 5] FIG. 5 is a typical metal structure photograph of Example 5 of the ultra-high hole expandability steel according to the present invention. [Figure 6] FIG. 6 is a typical metal structure photograph of Example 7 of the ultra-high hole-expandability steel according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0043] Referring to Figs. 1 to 3, a method for producing a full bainite type ultra-high hole expandability steel having a strength of 980 MPa according to the present invention includes the following steps: 1) Smelting and casting Smelting in a converter or electric furnace according to the composition described, followed by secondary refining in a vacuum furnace, then casting into billets or ingots; 2) Reheat the billet or ingot at a heating temperature of 1100 to 1200°C and a heat retention time of 1 to 2 hours; 3) Hot rolling The rolling start temperature is 950-1100°C, and 3-5 passes are performed under high rolling pressure at 950°C or higher, and the cumulative deformation amount is ≧50%; then, the intermediate billet temperature is 930-950°C, and 5-7 passes of finish rolling are performed, and the cumulative deformation amount is ≧70%; the rolling end temperature is 800-930°C; 4) Cooling First, air-cool for 0 to 10 seconds to allow dynamic recovery and dynamic recrystallization, then water-cool, and then heat the material to the bainite transformation temperature range, i.e., B s ~B f Water-cool the steel strip at a cooling rate of ≥ 10°C / s during the coiling process, then accelerate the cooling of the steel coil to room temperature by air-cooling (cooling rate > 20°C / h); 5) Pickling The pickling speed of the strip steel is adjusted in the range of 30-100 m / min, the pickling temperature is controlled between 75-85°C, the tensile straightening rate is controlled to be ≦2%, and the steel is rinsed at a temperature range of 35-50°C, and the surface is dried and oiled at a temperature range of 120-140°C.

[0044] The composition of the embodiment of the ultra-high hole expandability steel of the present invention is shown in Table 1, and the production process parameters of the embodiment of the steel of the present invention are shown in Tables 2 and 3, where the thickness of the steel billet in the rolling process is 230 mm; the mechanical properties of the steel plate of the embodiment of the present invention are shown in Table 4. The tensile properties (yield strength, tensile strength, elongation) were measured according to the ISO 6892-2-2018 international standard, the hole expansion ratio was measured according to the ISO 16630-2017 international standard, and the impact energy was measured according to the ISO 14556-2015 international standard.

[0045] As can be seen from Table 4, the steel coils all have a yield strength of ≥800MPa, a tensile strength of ≥980MPa, an elongation of typically ≥10%, a relatively stable impact energy, a -40°C low-temperature impact energy of ≥40J, and a hole expansion ratio of ≥60%. As can be seen from the above examples, the 980MPa high-strength steel of the present invention has excellent strength, plasticity, toughness and hole expansion compatibility, and is particularly suitable for the manufacture of parts such as control arms and other automobile chassis that require high strength, thinning and hole expansion and flanging, and can also be applied to parts such as wheels that require hole flanging and are complex to form, and is expected to be widely used.

[0046] [Table 1]

[0047] [Table 2]

[0048] [Table 3]

[0049] [Table 4]

Claims

1. The chemical composition, in weight percentage, is as follows: C 0.05-0.10%, Si≦2.0%, Mn 1.0-2.0%, P≦0.02%, S≦0.003%, Al 0.02-0.08%, N≦0.004%, Mo 0.1-0.5%, Ti 0.01-0.05%, O≦0.0030%, and the balance being Fe and other unavoidable impurities. An ultra-high hole expandability hot-rolled steel sheet having a tensile strength of 980 MPa or more and a fine structure of all bainite.

2. 2. The ultra-high hole expandability hot-rolled steel sheet having a tensile strength of 980 MPa or more and a microstructure of all bainite according to claim 1, further comprising one or more elements selected from the group consisting of Cr≦0.5%, B≦0.002%, Ca≦0.005%, Nb≦0.06%, V≦0.05%, Cu≦0.5%, and Ni≦0.5%.

3. The element is The content of Nb is ≦0.03%; The content of V is ≦0.03%; The content of Cu is ≦0.3%; The content of Ni is ≦0.3%; The Cr content is 0.2-0.4%; The content of B is 0.0005 to 0.0015%; and The content of Ca is ≦0.002%; The ultra-high hole-expandability hot-rolled steel plate having a tensile strength of 980 MPa or more and a microstructure of all bainite according to claim 2, further satisfying one or more of the following characteristics.

4. The ultra-high hole expandability hot-rolled steel sheet having a tensile strength of 980 MPa or more and a microstructure of all bainite according to claim 2, further comprising Cr≦0.5% and / or B≦0.002%.

5. The ultra-high hole expandability hot-rolled steel sheet having a tensile strength of 980 MPa or more and a fine structure of all bainite according to claim 1, wherein the C content is 0.06 to 0.09%.

6. The ultra-high hole expandability hot-rolled steel sheet having a tensile strength of 980 MPa or more and a fine structure of all bainite according to claim 1, wherein the Mn content is 1.4 to 1.8%.

7. The ultra-high hole expandability hot-rolled steel sheet having a tensile strength of 980 MPa or more and a microstructure of all bainite according to claim 1, wherein the S content is controlled to 0.0015% or less, and / or the N content is controlled to 0.003% or less.

8. The ultra-high hole expandability hot-rolled steel sheet having a tensile strength of 980 MPa or more and a fine structure of all bainite according to claim 1, wherein the Al content is 0.02 to 0.05%.

9. The ultra-high hole expandability hot-rolled steel sheet having a tensile strength of 980 MPa or more and a fine structure of all bainite according to claim 1, wherein the Ti content is 0.01 to 0.03% and / or the Mo content is 0.15 to 0.35%.

10. The ultra-high hole expandability steel has a yield strength of 800 MPa or more, a tensile strength of 980 MPa or more, and a lateral elongation A 50 The ultra-high hole expandability hot-rolled steel sheet having a tensile strength of 980 MPa or more and a fine structure of all bainite according to claim 1, wherein the tensile strength is ≥ 10%, and the hole expansion ratio is ≥ 60%.

11. An ultra-high hole-expandability hot-rolled steel plate having a tensile strength of 980 MPa or more and a fine structure of all bainite as described in claim 10, and having a -40°C impact toughness of ≧40J.

12. The ultra-high hole expandability hot-rolled steel sheet has a yield strength of ≥ 850 MPa, a tensile strength of ≥ 1020 MPa, and a transverse elongation A 50 ≧10%, hole expansion ratio ≧70%, and −40 ° C. impact toughness ≧50 J. The ultra-high hole expandability hot-rolled steel sheet having a tensile strength of 980 MPa or more and a fine structure of all bainite according to claim 10.

13. The ultra-high hole expandability hot-rolled steel sheet has a yield strength of ≧830 MPa, a tensile strength of ≧1000 MPa, and a transverse elongation A 50≧10%, hole expansion ratio ≧70%, and −40 ° C. impact toughness ≧60 J. The ultra-high hole expandability hot-rolled steel sheet having a tensile strength of 980 MPa or more and a fine structure of all bainite according to claim 10.

14. The ultra-high hole expandability hot-rolled steel sheet has a yield strength of ≧900 MPa, a tensile strength of ≧1040 MPa, and a transverse elongation A 50 ≧10%, hole expansion ratio ≧65%, and −40 ° C. impact toughness ≧40J. The ultra-high hole expandability hot-rolled steel sheet having a tensile strength of 980 MPa or more and a fine structure of all bainite according to claim 10.

15. A method for producing an ultra-high hole expandability hot-rolled steel sheet having a tensile strength of 980 MPa or more and a fine structure of all bainite according to any one of claims 1 to 14, comprising the following steps. 1) Smelting and casting smelting in a converter or electric furnace according to the composition according to any one of claims 1 to 9, followed by secondary refining in a vacuum furnace, followed by casting into billets or ingots; 2) Reheat the billet or ingot at a heating temperature of 1100 to 1200°C and a heat retention time of 1 to 2 hours; 3) Hot rolling The rolling start temperature is 950-1100°C, and 3-5 passes are performed under high pressure at 950°C or more, and the cumulative deformation amount is ≧50%; then, the intermediate billet temperature is 930-950°C, and 5-7 passes are performed for finish rolling, and the cumulative deformation amount is ≧70%; the rolling end temperature is 800-930°C; 4) Cooling First, air-cool for 0-10 seconds to achieve dynamic recovery and dynamic recrystallization, then water-cool the steel strip at a cooling rate of ≧10°C / s to the bainite transformation temperature range, and then coil the steel strip. Then, air-cool the steel coil to room temperature; 5) Pickling The pickling speed of the strip is adjusted in the range of 30-100 m / min, the pickling temperature is controlled between 75-85° C., the tensile straightening rate is controlled to be ≦2%, and then rinsed, the strip surface is dried and oiled.

16. In step 3), 3 to 5 passes are performed at 950°C or higher under high pressure, and the cumulative deformation amount is ≧70%; In step 3), the finish rolling is performed 5 to 7 passes, and the cumulative deformation amount is ≧80%; In step 4), the bainite transformation temperature range is between B s and B f ; In step 4), the strip is water-cooled to the bainite transformation temperature range at a cooling rate of 10-60° C. / s; and In step 4), the cooling temperature is 410-550°C; The method for producing an ultra-high hole expandability hot-rolled steel sheet having a tensile strength of 980 MPa or more and a microstructure of all bainite according to claim 15, further satisfying one or more of the following characteristics.

17. 16. The method for producing an ultra-high hole expandability hot-rolled steel sheet having a tensile strength of 980 MPa or more and a microstructure of all bainite according to claim 15, characterized in that after the pickling in step 5), rinsing is performed in a temperature range of 35 to 50 ° C, and the surface of the steel strip is dried and oiled at a temperature range of 120 to 140 ° C.

Citation Information

Patent Citations

  • High strength steel sheet having excellent weldability and hole expansibility and production method therefor

    JP2003193194A

  • Steel material and impact-absorbing member

    JP2012255176A

  • Hot-rolled steel sheet of high-formability and high-strength and method of manufacturing same

    KR1020150017252A