Cu-Ni-Al copper alloy sheet material, its manufacturing method and conductive spring member
By aligning Ni3Al-based precipitates in a specific orientation within Cu-Ni-Al copper alloys through controlled manufacturing, the etching rate is enhanced, addressing the slow etching issue and improving productivity.
Patent Information
- Application Number
- JP2021012409
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-01-28
- Publication Date
- 2024-12-05
- Estimated Expiration
- 2041-01-28
AI Technical Summary
Cu-Ni-Al based copper alloys used in conductive spring members face slow etching speeds, which hinder productivity due to the slow dissolution of the matrix and detachment of Ni-Al based precipitates during etching.
The formation of Ni3Al-based precipitates with a regular structure is aligned in a specific orientation to the plate surface, controlled through precise manufacturing conditions, including specific chemical composition and processing steps like solution treatment, aging treatment, and final cold rolling, to enhance the etching rate.
The etching rate of Cu-Ni-Al based copper alloy sheets is significantly improved, achieving a higher dissolution rate of the matrix and detachment of precipitates, resulting in enhanced productivity.
Smart Images

Figure 0007594923000001 
Figure 0007594923000002 
Figure 0007594923000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a Cu-Ni-Al-based copper alloy sheet material having an improved etching rate during part processing, a method for producing the same, and a conductive spring member using the sheet material. [Background technology]
[0002] Cu-Ni-Al copper alloys can be strengthened by Ni-Al precipitates, and have a metallic appearance close to white silver among copper alloys. Copper alloys with this composition are useful as conductive spring components such as lead frames, connectors, and leaf springs for VCM actuators, as well as non-magnetic high-strength components. However, in order to achieve high strength and excellent discoloration resistance, it is necessary to contain a large amount of Ni and Al. Therefore, high-strength Cu-Ni-Al copper alloy sheets suitable for thin-walled parts have a problem of low productivity due to the slow etching rate in the etching process performed when manufacturing parts.
[0003] Various studies have been conducted to date on improving the other properties of Cu-Ni-Al alloys while taking advantage of their high strength properties. For example, Patent Document 1 discloses a technique for obtaining a material having excellent strength, workability, and electrical conductivity by precipitating a γ' phase containing Si with an average grain size of 100 nm or less in a Cu-Ni-Al-based copper alloy containing a predetermined amount of Si through a process of performing a solution treatment at 700 to 1,020° C. and an aging treatment at 400 to 650° C. However, Patent Document 1 does not disclose any technique effective for improving the etching rate.
[0004] Patent Document 2 discloses a manufacturing technique for a plate material with excellent etching properties in a Cu-Ni-Al-based copper alloy. In the manufacturing process, rapid heating is performed during solution treatment, cold rolling is performed after aging treatment, and then a finishing heat treatment is performed so that the heating rate is not excessive. This results in a structure state with a large KAM value, and a highly smooth etched surface is obtained. It is also taught that reducing the generation of coarse precipitates is also effective in forming a highly smooth etched surface. However, the technique disclosed in Patent Document 2 does not sufficiently improve the etching rate.
[0005] Patent Document 3 discloses a technique for manufacturing a Cu-Ni-Al-based copper alloy plate material that has an excellent "strength-bending workability balance" and excellent discoloration resistance. In the manufacturing process, a method is adopted in which a material that has been subjected to a solution treatment is given cold rolling strain as necessary, and then a first aging treatment at a higher temperature range and a second aging treatment at a conventionally general temperature range are successively performed. This two-stage aging treatment makes it difficult for discontinuous precipitation of grain boundary reaction to occur, and sufficient intragranular precipitation of fine second phase particles that contribute to strength improvement occurs, thereby achieving an excellent strength-bending workability balance. However, Patent Document 3 does not disclose a technique that is effective for improving the etching rate.
[0006] Patent Document 4 discloses a manufacturing technology for a plate material having a high Young's modulus in a Cu-Ni-Al-based copper alloy. Specifically, a specific crystal orientation is obtained by performing cold rolling with intermediate annealing under specific conditions, performing solution treatment at a slow heating rate, and performing finish cold rolling under conditions where the rolling reduction ratio is controlled to be low, followed by aging treatment, thereby realizing a high Young's modulus. However, Patent Document 4 does not disclose any technology that is effective in improving the etching rate.
[0007] Patent Document 5 discloses a technique for improving the strength and bending workability of a Cu-Ni-Al-based copper alloy containing 15% or less by weight of Ni and 2% or less by weight of Al. However, there is no mention of the etching rate. In the technique of Patent Document 5, a decrease in the etching rate can be a problem, particularly in a Cu-Ni-Al-based copper alloy containing a large amount of Ni and Al and having high strength and excellent discoloration resistance. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] International Publication No. 2012 / 081573 [Patent Document 2] JP 2019-2042 A [Patent Document 3] JP 2020-50923 A [Patent Document 4] JP 2020-79436 A [Patent Document 5] Japanese Patent Application Publication No. 5-320790 Summary of the Invention [Problem to be solved by the invention]
[0009] Although Cu-Ni-Al based copper alloy sheet materials are useful for conductive spring members such as connectors, they have a problem of slow etching rate. The present invention aims to provide a Cu-Ni-Al based copper alloy sheet material with an improved etching rate. [Means for solving the problem]
[0010] In Cu-Ni-Al copper alloys, Ni-Al precipitates mainly composed of Ni3Al intermetallic compounds with an L12 ordered structure (hereinafter sometimes referred to as "Ni3Al precipitates") are generated during the manufacture of the sheet material. Among these precipitates, fine precipitate particles with a major axis of 5 to 50 nm in particular contribute to high strength, but many precipitate particles with a major axis exceeding 50 nm are also generated. In order to improve the etching rate of Cu-Ni-Al copper alloy sheets, it is important that (i) the dissolution rate of the parent phase (metal base) in the etching solution is high, and (ii) the Ni-Al precipitates are likely to be detached from the parent phase during etching. According to the inventors' research, in order to achieve these (i) and (ii), it is extremely advantageous that the crystal orientation of the Ni-Al precipitates with respect to the sheet surface (rolled surface) is aligned in a certain direction as much as possible, and that Ni-Al precipitates with a high degree of order (i.e., an atomic arrangement as close as possible to the L12 ordered structure) are present in as large an amount as possible. Such a metal structure is characterized by the X-ray diffraction intensity ratio X A It was also confirmed that a sheet material having such a metal structure can be industrially produced by strictly controlling the production conditions. The present invention is based on these findings.
[0011] In this specification, "plate material" refers to a sheet-like metal material formed by utilizing the malleability of metal. Thin sheet-like metal materials are sometimes called "foils", and such "foils" are also included in the "plate material" referred to here. Long sheet-like metal materials wound into a coil are also included in the "plate material". In this specification, the thickness of a sheet-like metal material is called the "plate thickness". Also, the "plate surface" is the surface perpendicular to the plate thickness direction of the plate material. The "plate surface" is also called the "rolled surface".
[0012] The object of the present invention is to provide a sheet having a chemical composition, in mass%, of 10.0-30.0% Ni, 1.0-6.5% Al, 0-0.5% Ag, 0-0.1% B, 0-0.15% Be, 0-2.0% Co, 0-0.5% Cr, 0-0.5% Fe, 0-2.0% Ga, 0-0.5% Ge, 0-0.5% In, 0-0.5% Mg, 0-0.5% Mn, 0-2.0% P, 0-0.2% Si, 0-0.8% Sn, 0-2.0% Ti, 0-2.0% Zn, 0-2.0% Zr, and the balance being Cu and unavoidable impurities, which satisfies the following formula (1), and in the X-ray diffraction pattern of the sheet surface, the X-ray diffraction pattern of the following formula (2) is obtained. A The value is 1.5 x 10 -3 The above-mentioned object is achieved by the copper alloy sheet material. Ni / Al≦9.0 …(1) Here, the content value of the element expressed as mass% is substituted for the element symbol in formula (1). X A =I{110} / (I{111}+I{200}+I{220}+I{311}+I{331}+I{420}) …(2) Here, I{110} is the integrated intensity of the diffraction peak of the {110} crystal plane of the Ni3Al-type precipitate, and the other I{hkl} is the integrated intensity of the diffraction peak that is a superposition of the diffraction peak of the {hkl} crystal plane of the parent phase and the {hkl} crystal plane of the Ni3Al-type precipitate.
[0013] The above plate material has an X-ray diffraction intensity ratio X according to the following formula (3). B The value is, for example, 0.20 or more. X B =I{220} / (I{111}+I{200}+I{220}+I{311}+I{331}+I{420}) …(3) Here, I{hkl} is the integrated intensity of the diffraction peak that is the superposition of the diffraction peak of the parent phase {hkl} crystal plane and the diffraction peak of the Ni3Al-type precipitate {hkl} crystal plane.
[0014] In the above copper alloy sheet, the number density of coarse precipitate particles with a major axis of 1 μm or more on an observation surface parallel to the sheet surface is 3.0 × 10 4 pieces / mm 2It is preferable that: The number density of fine precipitate particles with a long diameter of 5 to 50 nm in the observation plane parallel to the plate surface is 1.0 × 10 7 pieces / mm 2 More preferably, it is equal to or greater than this. The tensile strength in the rolling direction is preferably 900 MPa or more. The copper alloy sheet has a thickness of, for example, 0.02 to 0.40 mm.
[0015] The copper alloy sheet material can be obtained by the following manufacturing method. A step of heating the slab having the above chemical composition at 1000 to 1150°C (slab heating step); A process of performing hot rolling under conditions in which the rolling temperature in the final rolling pass is 800°C or higher (hot rolling process); Cold rolling process (cold rolling process) 5~25N / mm 2 a process of holding the material at 950 to 1100°C for 30 to 360 seconds while applying a tension of 100°C, and then cooling the material at an average cooling rate of 80°C / s or more from 900°C to 300°C (solution treatment process); A process of increasing the temperature from 300°C to 400°C at an average heating rate of 40°C / h or more and holding the temperature at 400 to 650°C for 0.1 to 75 hours (aging treatment process); A process of performing cold rolling with a total rolling reduction of 40% or more using a pass schedule including four or more rolling passes with a rolling reduction of 12% or more per pass (final cold rolling process); 70~150N / mm 2 A process of holding the sheet at 400 to 700°C for 10 to 600 seconds while applying a tension (final heat treatment process); In the above order, the manufacturing process includes the steps of: A The value is 1.5 x 10 -3 A method for producing a copper alloy sheet material, which obtains the above-mentioned sheet material. In addition, the X-ray diffraction intensity ratio X according to the above formula (3) B The plate material may have a value of 0.20 or more.
[0016] The thickness of the plate material obtained in the final cold rolling step can be, for example, 0.02 to 0.40 mm.
[0017] The present invention also provides a conductive spring member using the above-mentioned copper alloy sheet material as its material.
[0018] The X-ray diffraction intensity ratio X of the above formula (2) A The value can be calculated as follows: [X-ray diffraction intensity ratio X A How to calculate the value For the sheet surface (rolled surface), an X-ray diffraction pattern including a range of diffraction angles 2θ of 30 to 150° is measured using an X-ray diffractometer under the conditions of Cu-Kα radiation, tube voltage 30 kV, tube current 10 mA, measurement step 0.04°, and measurement time per step 1 second. However, if the S / N ratio of the obtained X-ray diffraction pattern is less than 1.5, the measurement time per step is set to 10 seconds. Here, the S / N ratio is the value obtained by dividing the signal by the noise, where the peak intensity of the {110} peak after removing Kα radiation is the signal (unit: cps) and the difference between the maximum and minimum values of the X-ray intensity in the range of 2θ of 110 to 115° is the noise (unit: cps). The measurement is performed while rotating the sample at 30 revolutions per minute with the plate thickness direction as the rotation axis. Based on the obtained X-ray diffraction pattern data, the Kα2 radiation is removed using X-ray diffraction pattern analysis software, and then fitting is performed with a pseudo Voigt function to determine the integrated intensity I{hkl} of each {hkl} peak. The value of each I{hkl} is substituted into the following formula (2) to obtain the X-ray diffraction intensity ratio X A Calculate the value. X A =I{110} / (I{111}+I{200}+I{220}+I{311}+I{331}+I{420}) …(2) Here, the misfit of the lattice constant between the parent phase, which is the metal base, and the Ni3Al intermetallic compound with the L12 type ordered structure is small at about 0.75%, so the {hkl} diffraction peaks of both appear superimposed in the X-ray diffraction pattern. However, since the parent phase has an fcc structure (face-centered cubic lattice), no diffraction peaks appear for crystal planes in which the indices h, k, and l are a mixture of even and odd numbers. Therefore, the {110} peaks appearing in the X-ray diffraction pattern are diffraction peaks from the precipitates only. That is, in the above formula (2), I{110} is the integrated intensity of the diffraction peak of the {110} crystal plane of the Ni3Al type precipitate, and the other I{hkl} is the integrated intensity of the diffraction peak in which the diffraction peak of the parent phase {hkl} crystal plane and the diffraction peak of the Ni3Al type precipitate {hkl} crystal plane are superimposed.
[0019] The X-ray diffraction intensity ratio X of the above formula (3) B The value is the "X-ray diffraction intensity ratio X A This can be calculated using a method similar to that described in "How to calculate the value of .
[0020] For reference, Table 1 shows examples of calculated values of diffraction angle 2θ using Cu-Kα radiation for the parent phase (fcc) of a Cu-Ni-Al based copper alloy and the Ni3Al intermetallic compound (L12).
[0021] [Table 1]
[0022] The "number density of coarse precipitate particles having a major axis of 1.0 μm or more" and the "number density of fine precipitate particles having a major axis of 5 to 50 nm" can each be determined as follows.
[0023] [How to determine the number density of coarse precipitate particles] The plate surface was electrolytically polished under the following electrolytic polishing conditions to dissolve only the Cu base material and expose the precipitate particles, which were then ultrasonically cleaned in ethanol for 20 minutes. The surface was then observed at a magnification of 2000x using a field emission scanning electron microscope (FE-SEM), and the total number of precipitate particles with a major axis of 1.0 μm or more observed on the FE-SEM image was calculated based on the total observation area (mm 2 ) is the particle number density of the coarse precipitate particles (particles / mm 2 ) where the longest diameter is the length of the longest line segment connecting any two points on the outer edge of a precipitate particle on the FE-SEM image. Observations are performed on at least 20 randomly set, non-overlapping fields of view. Precipitate particles that partially protrude from the observation field of view are counted if the longest diameter of the portion that appears within the observation field of view is 1.0 μm or more. (Electrolytic polishing conditions) Electrolyte: Distilled water, phosphoric acid, ethanol, and 2-propanol mixed in a ratio of 10:5:5:1 Liquid temperature: 20℃ Voltage: 15V ·Electrolysis time: 20 seconds
[0024] [How to determine the number density of fine precipitate particles] The plate surface is electrolytically polished under the electrolytic polishing conditions described below, and then ultrasonically cleaned in ethanol for 20 minutes to obtain an observation surface, which is observed at a magnification of 100,000 times using a FE-SEM (field emission scanning electron microscope). Observation fields are randomly selected that do not include any or all particles with a major axis of 1.0 μm or more. For each observation field, the number of precipitate particles with a major axis of 5 to 50 nm among particles whose entire outlines are visible is counted. This operation is performed for 10 or more observation fields with no overlapping areas, and the total number of counts in all observed fields is calculated as N TOTAL is divided by the total area of the observation field, and the result is 1 mm 2 This is converted to the number of fine precipitate particles per mm 2 ) (Electrolytic polishing conditions) Electrolyte: Distilled water, phosphoric acid, ethanol, and 2-propanol mixed in a ratio of 10:5:5:1 Liquid temperature: 20℃ Voltage: 15V ·Electrolysis time: 20 seconds
[0025] The rolling ratio from a certain plate thickness t0 (mm) to a certain plate thickness t1 (mm) is calculated by the following formula (4). Rolling ratio (%) = [(t0-t1) / t0] × 100 … (4) Effect of the Invention
[0026] According to the present invention, in a high-strength Cu-Ni-Al-based copper alloy sheet material having a composition range that exhibits a whitish metallic appearance, the etching rate can be significantly improved compared to the conventional method. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0027] [Chemical composition] The present invention is directed to a Cu-Ni-Al based copper alloy. Hereinafter, "%" regarding the alloy components means "mass %" unless otherwise specified.
[0028] Ni is a major element that, together with Cu, constitutes the matrix (metal base) of Cu-Ni-Al copper alloys. In addition, a part of Ni in the alloy combines with Al to form Ni-Al precipitates, and the fine particles contribute to improving strength. In order to obtain sufficient strength, it is desirable to ensure a Ni content of 10.0% or more. In addition, as the Ni content increases, the alloy exhibits a whiter metallic appearance compared to other general copper alloys. However, like other copper alloys, when exposed to a high humidity environment, a thin oxide film forms on the metal surface, which may cause noticeable discoloration. In that case, the beautiful white appearance is lost. In particular, when emphasis is placed on discoloration resistance, it is more preferable to increase the Ni content to 12.0% or more and ensure the Al content as described below. It is more effective to make the Ni content 15.0% or more. On the other hand, if the Ni content is high, the hot workability deteriorates. The Ni content is limited to 30.0% or less, and may be limited to 25.0% or less. The Ni content may be controlled to 18.0% or more and 22.0% or less.
[0029] Al is an element that forms Ni-Al precipitates. If the Al content is too low, the strength improvement is insufficient. On the other hand, if the Al content is too high, the hot workability deteriorates. Also, by increasing the Al content along with the increase in the Ni content, it is possible to improve discoloration resistance. As a result of various investigations, it has been found that the Al content must be in the range of 1.0 to 6.5%, and the Ni / Al ratio must satisfy the following formula (1). It is more preferable that the following formula (1)' is satisfied. Ni / Al≦9.0 …(1) 2.0≦Ni / Al≦8.0 …(1)' Here, the content value of the corresponding element expressed as mass % is substituted for the element symbol in formula (1) and formula (1)'.
[0030] Other elements such as Ag, B, Be, Co, Cr, Fe, Ga, Ge, In, Mg, Mn, P, Si, Sn, Ti, Zn, and Zr may be contained as necessary. The content ranges of these elements are Ag: 0-0.5%, B: 0-0.1%, Be: 0-0.15%, Co: 0-2.0%, Cr: 0-0.5%, Fe: 0-2.0%, Ga: 0-0.5%, Ge: 0-0.5%, In: 0-0.5%, Mg: 0-0.5%, Mn: 0-2.0%, P: 0-0.2%, Si: 0-0.8%, Sn: 0-2.0%, Ti: 0-2.0%, Zn: 0-2.0%, and Zr: 0-0.3%. The total amount of these optional added elements is desirably 2.0% or less, and may be 1.2% or less, or 1.0% or less, or even 0.5% or less.
[0031] [X-ray diffraction intensity ratio X A value] The copper alloy sheet material of the present invention has an X-ray diffraction intensity ratio X A The value is 1.5 x 10 -3 The above is the requirement. X A =I{110} / (I{111}+I{200}+I{220}+I{311}+I{331}+I{420}) …(2) Here, I{110} is the integrated intensity of the diffraction peak of the {110} crystal plane of the Ni3Al-type precipitate as described above, and the other I{hkl} is the integrated intensity of the diffraction peak in which the diffraction peak of the parent phase {hkl} crystal plane and the diffraction peak of the Ni3Al-type precipitate {hkl} crystal plane are superimposed.
[0032] According to the research of the inventors, in the case of a Cu-Ni-Al based copper alloy sheet material, the above X A The value is 1.5 x 10 -3 It was found that when the structure was adjusted to the above condition, the etching property was significantly improved. A The value is 2.0 x 10 -3 More preferably, it is 2.5×10 or more. -3 More preferably, it is 5.0×10 or more. -3 More than this is more effective. A There is no particular upper limit to the value, but in the composition defined in the present invention, X A For example, the value is 50.0×10 -3 It is sufficient to control it within the following range.
[0033] In the Cu-Ni-Al based copper alloy sheet material according to the present invention, A The value is higher than the previous one. X A The reasons for the high value include the following: (a) The amount of Ni-Al precipitates formed is large. (b) The Ni-Al precipitates that have formed have a high degree of orientation of the {110} crystal plane of the Ni3Al precipitates on the sheet surface (rolled surface). (c) There are many Ni-Al-based precipitate particles with a high degree of order (i.e., an atomic arrangement as close as possible to the L12 type ordered structure).
[0034] The etching of Cu-Ni-Al-based copper alloy sheet material is considered to proceed mainly by "dissolution of the parent phase" and "detachment of precipitates". A It is presumed that the above factors (a) to (c) that increase the value contribute to the improvement of the etching rate through the following actions. Regarding (a) A large amount of precipitates means that the amount of solute atoms (Ni, Al) dissolved in the parent phase is small. One of the main reasons for the slow etching rate of Cu-Ni-Al copper alloys is the high concentration of solute atoms in the parent phase. The small amount of solute atoms in the parent phase is advantageous for improving the dissolution rate of the parent phase. In addition, a large amount of precipitates is also effective in promoting etching through "detachment of precipitates." Regarding (b) It is believed that if the crystal orientation of the precipitates is aligned in a certain direction that makes it relatively easy for them to be detached from the parent phase, this is advantageous for improving the etching rate. The inventors believe that the high degree of orientation of the {110} crystal plane of the Ni3Al type precipitates to the sheet surface (rolled surface) is one of the factors that promotes the detachment of the precipitates. Regarding (c) It is presumed that when the degree of ordering of precipitates is low, the properties of the precipitates become closer to those of the parent phase, making it difficult for the precipitates to detach from the parent phase. Therefore, it is believed that a high degree of ordering of precipitates contributes to promoting the detachment of the precipitates.
[0035] [X-ray diffraction intensity ratio X B value] The above X A The value is an index related to the amount of precipitates and the crystal orientation. In addition to this, the X-ray diffraction intensity ratio X, calculated by the following formula (3), is used as an index for identifying the crystal orientation of the parent phase (metallic base), i.e., the texture. B The value can be given. X B =I{220} / (I{111}+I{200}+I{220}+I{311}+I{331}+I{420}) …(3) Here, I{hkl} is the integrated intensity of the diffraction peak that is the superposition of the diffraction peak of the parent phase {hkl} crystal plane and the diffraction peak of the Ni3Al-type precipitate {hkl} crystal plane.
[0036] In the Cu-Ni-Al based copper alloy sheet material according to the present invention, the above X BThe microstructure state in which the value is 0.20 or more is obtained. Since the misfit (difference in lattice constant) between the Ni3Al type precipitates and the parent phase is small, it is considered that the Ni3Al type precipitates, which are large in size, also have a high degree of coherence with the parent phase. A It is presumed that the strong orientation of the {110} parent phase plane to the sheet surface (rolled surface) is advantageous in increasing the value above a certain level. The orientation of the {110} parent phase plane is grasped by the relative diffraction intensity I{220} of the {220} parent phase plane in the X-ray diffraction pattern. The index representing this is the X-ray diffraction intensity ratio X, determined by equation (3): B The value is X. B The value should be 0.20 or more, and preferably 0.30 or more. In the plate material having the composition specified in the present invention, X B Values will be in the range of 0.80 or less.
[0037] For reference, the integrated intensities of the diffraction peaks calculated from the X-ray diffraction pattern of the sheet material of the present invention obtained in Example No. 4 described later are shown below. Crystal plane index Integrated intensity of diffraction peak {110} 63.5 {111} 485.1 {200} 42.1 {220} 1565.8 {311} 70.5 {331} 506.2 {420} 158.1 In this example, the X-ray diffraction intensity ratio X A Value = 63.5 / (485.1+42.1+1565.8+70.5+506.2+158.1) ≒ 22.5 × 10 -3 It is calculated as follows. In addition, the X-ray diffraction intensity ratio X B The value is calculated as 1565.8 / (485.1+42.1+1565.8+70.5+506.2+158.1) ≒ 0.55.
[0038] [Number density of coarse precipitate particles with major axis of 1.0 μm or more] In order to form a smooth etched surface by etching, it is advantageous to minimize the amount of coarse precipitates. Specifically, the density of coarse precipitate particles with a major axis of 1.0 μm or more is 3.0 × 10 4 pieces / mm 2 It is preferable that the value is less than 1.0×10 4 pieces / mm 2 It is more preferable that:
[0039] [Number density of fine precipitate particles with major axis of 5 to 50 nm] In order to realize high-strength Cu-Ni-Al-based copper alloy sheet, the number density of fine precipitate particles with a long diameter of 5 to 50 nm on an observation surface parallel to the sheet surface must be 1.0 × 10 7 pieces / mm 2 More preferably, it is 2.0×10 7 pieces / mm 2 When emphasis is placed on increasing strength, the number density of fine precipitate particles having a major axis of 5 to 50 nm is preferably set to 4.0×10 or more. 7 pieces / mm 2 More than 6.0×10 is effective. 7 pieces / mm 2 It is more effective to set the number density to 15.0×10 or more. However, in order to have a large amount of fine precipitate particles, the composition and manufacturing conditions are subject to strict restrictions. The number density of fine precipitate particles with a major axis of 5 to 50 nm is usually 15.0×10 7 pieces / mm 2 The adjustment may be made within the following range.
[0040] [Tensile strength] For application to high-strength current-carrying spring members, the tensile strength in the rolling direction is preferably 900 MPa or more, more preferably 1000 MPa or more, and can be adjusted to 1300 MPa or more.
[0041] [Manufacturing method] The copper alloy sheet material described above can be produced, for example, by the following manufacturing process. Casting → heating of the slab → hot rolling → cold rolling → (intermediate annealing → cold rolling) → solution treatment → aging treatment → final cold rolling → final heat treatment Although not described in the above steps, facing is performed as necessary after hot rolling, and pickling, polishing, or further degreasing is performed as necessary after each heat treatment. Each step will be described below.
[0042] [casting] The cast pieces may be produced by continuous casting, semi-continuous casting, etc. From the viewpoint of preventing oxidation of Al, it is preferable to carry out melting in a chamber under an inert gas atmosphere or under vacuum.
[0043] [Slab heating] The slab is heated and held at 1000 to 1150° C. It is effective to hold the slab for 1.5 hours or more in this temperature range, and more preferably for 2 to 5 hours, and then the slab is removed from the furnace and hot-rolled.
[0044] [Hot rolling] In hot rolling, the rolling temperature of the final pass is set to 800°C or higher. The temperature of each rolling pass can be expressed by the surface temperature of the material immediately after it leaves the work roll in that rolling pass. The above-mentioned heating of the slab and hot rolling at 800°C or higher can reduce the amount of coarse second phases (Ni-Al-based precipitate phases), and ultimately produce a plate material with a low number density of coarse precipitates. In addition, the reduction of the coarse second phases at this stage can be achieved by maintaining the above-mentioned X value, which is sufficiently high, in the final plate material. A From the viewpoint of stably achieving a final pass rolling temperature of 800° C. or more in mass production operations, the plate thickness after hot rolling (finished plate thickness) is preferably in the range of, for example, 5 to 20 mm, and more preferably in the range of 7 to 20 mm.
[0045] [Cold rolling] It is desirable to adjust the plate thickness by cold rolling before the solution treatment. If necessary, the process of "intermediate annealing → cold rolling" may be added once or more. The reduction ratio in the cold rolling performed before the solution treatment (if intermediate annealing is performed, the reduction ratio in the cold rolling after the final intermediate annealing) can be, for example, 80% or more. The upper limit of the reduction ratio may be set, for example, in the range of 99.5% or less depending on the capacity of the mill. In this way, an intermediate product plate material to be subjected to the solution treatment can be prepared. The plate thickness of the material to be subjected to the solution treatment is preferably, for example, 0.20 to 0.60 mm.
[0046] [Solution treatment] In the solution treatment of the present invention, Ni and Al existing as second phases are sufficiently dissolved and an appropriate residual stress is introduced. The introduction of this residual stress has the effect of facilitating the formation of precipitate particles in which the {110} crystal plane of Ni3Al type precipitates is roughly parallel to the rolled surface (hereinafter, referred to as "{110} / / rolled surface precipitate particles"). In order to achieve sufficient solution and introduce an appropriate residual stress, in the present invention, solution treatment is performed under strict condition control, in which solution treatment is performed at a relatively high temperature while applying a tension in a specified range, and then the material is rapidly cooled.
[0047] Specifically, the time for which the material is held in the temperature range of 950 to 1100°C is set to 30 to 360 seconds, and the material is subjected to a force of 5 to 25 N / mm 2The tension is applied. The tension can be controlled, for example, by the driving force of the bridle rolls at both ends of the heating zone while the sheet is passing through a continuous heat treatment furnace. The direction of the tension is the rolling direction. When the sheet is heated to the high temperature range as described above, the second phase can be sufficiently dissolved even if the holding time is relatively short. If the tension is too low, the residual stress is insufficient, and the precipitate particles on the {110} / / rolled surface cannot be sufficiently generated in the aging treatment process. If the tension is too high, the residual stress becomes excessive, and the precipitate particles on the {110} / / rolled surface may not be stably and sufficiently generated in the subsequent aging treatment process. After the heating and holding, the sheet is cooled under conditions where the average cooling rate from 900°C to 300°C is 80°C / s or more. If this cooling rate is too slow, the nucleation and growth of the precipitate particles occurs more than necessary during the cooling process, and in this case too, it becomes difficult to sufficiently generate the precipitate particles on the {110} / / rolled surface in the subsequent aging treatment process.
[0048] [Aging process] Following the solution treatment, aging treatment is performed. In this aging treatment, the average heating rate from 300°C to 400°C is set to 40°C / h or more in order to reach the precipitation temperature before the residual stress introduced by the solution treatment is recovered. After that, the material is held at 400-650°C for 0.1-75 hours, and then cooled. This makes it possible to control the orientation of the precipitates, and to realize an aged structure rich in precipitate particles on the {110} / / rolled surface.
[0049] At the end of this aging treatment, compared to the conventional manufacturing method, X A Although the value is improved, it is not enough to achieve a sufficient improvement in the etching rate. After this, final cold rolling and final heat treatment are performed to reduce the X A The etching rate will be further improved by further increasing the value.
[0050] [Final cold rolling] After the aging treatment, cold rolling is performed to the final target plate thickness. This cold rolling is referred to as "final cold rolling" in this specification. The plate thickness after the final cold rolling is preferably adjusted to, for example, a range of 0.02 to 0.40 mm. The plate thickness may be set to a range of 0.25 mm or less. It is also possible to obtain a very thin plate material of 0.10 mm or less.
[0051] In order to fully advance the {110} / / rolled surface orientation of the precipitate particles in the final cold rolling process, it is effective to perform cold rolling with a total rolling reduction of 40% or more in a pass schedule that includes four or more rolling passes with a rolling reduction of 12% or more per pass. It is presumed that this method will efficiently advance the {110} / / rolled surface orientation of the precipitate particles. If this orientation is insufficient, the X A The upper limit of the total rolling ratio may be set in the range of, for example, 99% or less depending on the capacity of the mill.
[0052] [Final heat treatment] After the final cold rolling, the plate material is subjected to final heat treatment. A This heat treatment aims to further improve the strength of the material. 2 The rolling is carried out under the condition of holding the sheet at 400 to 700°C for 10 to 600 seconds while applying a tension of 100 mm. The tension can be controlled, for example, by the driving force of the bridle rolls at both ends of the heating zone while the sheet is passed through a continuous heat treatment furnace. It is believed that the application of the above-mentioned predetermined tension generates a large number of precipitate particles on the {110} / / rolled surface, and finally, the X A The tissue condition is such that the value is sufficiently high. A In addition to controlling the value, strict tension control is also required to obtain the shape correction effect by the final heat treatment. By applying the above-mentioned predetermined tension, a thin plate material with a good shape can be obtained, which has the property of obtaining high dimensional accuracy when processed into precision parts.
[0053] The plate material according to the present invention obtained as described above can be used as a starting material and processed, including etching, to efficiently obtain conductive spring members with high dimensional accuracy. EXAMPLES
[0054] Copper alloys having the chemical compositions shown in Table 2 were melted and cast using a vertical semi-continuous casting machine. The resulting slabs were heated and held at the temperatures and times shown in Tables 3 and 4, then extracted, hot rolled, and water-cooled. The total hot rolling reduction was 75-98%. The rolling temperature of the final pass and the finished plate thickness after hot rolling are shown in Tables 3 and 4. In some cases (Nos. 36, 37, and 38) where cracks occurred during hot rolling, production was discontinued at that point. After hot rolling, the oxide layer on the surface was removed by mechanical polishing (face grinding), and cold rolling to the rolling ratios shown in Tables 3 and 4 was performed.
[0055] The obtained cold-rolled materials were subjected to solution treatment under the conditions shown in Tables 3 and 4 using a continuous annealing furnace equipped with a heating zone and a forced cooling zone. In the heating zone, the material was heated at a predetermined temperature for a predetermined time while being applied with a predetermined tension by the driving force of the bridle rolls at both ends of the heating zone. Then, in the forced cooling zone, forced cooling was performed by blowing nitrogen gas forcedly circulated by a fan onto the surface of the plate during passing. The cooling rate can be controlled by adjusting the convection strength. During the passing, the material surface temperature T0 (℃) just before the start of forced cooling and the material surface temperature T1 (℃) just after the end of forced cooling were measured. It was confirmed that T0 was 900℃ or higher and T1 was 300℃ or lower in each example. Therefore, the average cooling rate from 900℃ to 300℃ was calculated based on the cooling curve determined from the above T0, T1, and the passing speed.
[0056] After the solution treatment, the steel was directly subjected to aging treatment without applying cold rolling strain. The aging treatment was performed using a batch-type annealing furnace under the conditions of holding the temperatures and times shown in Tables 3 and 4 for the times shown in the same tables. The atmosphere was nitrogen. During the temperature rise in the aging treatment, the average heating rate from 300°C to 400°C was controlled. After holding at the temperature, the steel was cooled in the furnace at a roughly constant cooling rate until the temperature became lower than 300°C. Then, final cold rolling was performed under the conditions shown in Tables 3 and 4 to obtain the final plate thickness shown in the same tables. The column "≧12% number of passes" in Tables 3 and 4 shows the number of rolling passes in which the rolling ratio per pass was 12% or more. The strips were then subjected to final heat treatment under the conditions shown in Tables 3 and 4 in a continuous annealing furnace equipped with a heating zone and a forced cooling zone. In the heating zone, the strips were heated at a specified temperature for a specified time while being subjected to a specified tension by the driving force of bridle rolls at both ends of the heating zone. After leaving the heating zone, the strips were forced to cool in the forced cooling zone by blowing nitrogen gas forced by a fan onto the strip surface as it was passing through.
[0057] In this manner, plate products (test materials) were obtained having the final thicknesses shown in Tables 3 and 4. The following investigations were carried out on each test material.
[0058] (X-ray diffraction intensity ratio X A value) The X-ray diffraction intensity ratio X A According to the method for calculating the X-ray diffraction intensity ratio X, the X-ray diffraction pattern of the plate surface (rolled surface) of a sample (20 mm × 20 mm) cut from each test material was measured using an X-ray diffractometer (D2 Phaser 2nd Generation, manufactured by Burker AXS). After removing the Cu-Kα2 line from the X-ray diffraction pattern, the integrated intensity I{hkl} of each {hkl} peak was calculated, and the X-ray diffraction intensity ratio X was calculated using the above formula (2). A The value was obtained. DIFFRAC.EVA (Ver.4.2.1.10) manufactured by Burker AXS was used to calculate the signal used for removing Cu-Kα2 radiation and calculating the S / N ratio. The conditions for removing Cu-Kα2 radiation were "Max: 1, Intensity ratio: 0.5, Min: 0". After removing Kα2 radiation, the background was removed in the range of 2θ from 30 to 40° under the conditions of "Curvature: 1.000, Threshold: 1.000" using the "Background" tool, and the {110} peak intensity (unit: cps) was calculated using the "Create area" tool to obtain the signal. Topas (Ver.5) manufactured by Burker AXS was used as the X-ray diffraction pattern analysis software. The integrated intensity I{110} of the {110} diffraction peak of Ni3Al type precipitates was calculated by fitting a pseudo Voigt function in the range of 2θ from 30° to 40° while changing Position (initial value: 35), Area (initial value: 50), and Cry size L (initial value: 10). For background processing, "Chebychev" and "1 / X Bkg" were used, and "Order" was set to 0. The Area value after performing fitting five times was taken as I{110}. Other I{hkl} were calculated by fitting with the initial value of Position set to the position of each {hkl} diffraction peak in the 2θ range of 40° to 150°, cry size L fixed to 200, and Position and Area changed. Background processing was performed using "Chebychev" with "Order" set to 1. The Area value of each {hkl} diffraction peak after one fitting was performed was taken as I{hkl}.
[0059] (X-ray diffraction intensity ratio X B value) Above X A Using the same method as the value, the X-ray diffraction intensity ratio X was calculated based on the X-ray diffraction pattern of each test material using the above formula (3). B The value was calculated.
[0060] (Number density of coarse precipitate particles) According to the above-mentioned "Method of determining the number density of coarse precipitate particles", the observation surface prepared by electrolytic polishing and ultrasonic cleaning was observed with an FE-SEM (JSM-7200F manufactured by JEOL Ltd.) to determine the number density of coarse precipitate particles with a major axis of 1.0 μm or more. The observation was performed at a magnification of 2000 times and in 20 fields of view. The electrolytic polishing was performed using an electrolytic polishing device (ElectroMet 4) manufactured by BUEHLER. The ultrasonic cleaning was performed in ethanol for 20 minutes using an ultrasonic cleaner "BRANSONIC M2800-J".
[0061] (Number density of fine precipitate particles) According to the above-mentioned "Method of determining the number density of fine precipitate particles", the observation surface prepared by electrolytic polishing and ultrasonic cleaning was observed with an FE-SEM (JSM-7200F manufactured by JEOL Ltd.), and the number density (particles / mm ) of fine second phase particles with a major axis of 5 to 50 nm was determined. 2 ) was obtained. Observation was performed at a magnification of 100,000 times, covering 10 fields of view. The electrolytic polishing was performed using an electrolytic polishing device manufactured by BUEHLER (ELECTROPOLISHER POWER SUPPLUY, ELECTROPOLISHER CELL MODULE). The ultrasonic cleaning was performed in ethanol for 20 minutes using an ultrasonic cleaner "BRANSONIC M2800-J."
[0062] (Tensile strength) Tensile test pieces (JIS No. 13 B) in the rolling direction (LD) were taken from the test material, and tensile tests were performed according to JIS Z2241 with the number of tests being n = 5 to measure the tensile strength. The average value of n = 5 was taken as the performance value of the test material.
[0063] (etching rate) A test piece with a width of about 10 mm and a length of about 50 mm was cut out from the test material, and the surface (rolled surface) was etched using a spray-type etching device. The thickness of the plate was measured before and after etching to determine the amount of thickness reduction. The etching solution was an aqueous solution of ferric chloride with a Baume scale of 42 Bh. The liquid temperature was 50°C, the spray pressure was 0.15 MPa, and the spray time was set so that the amount of thickness reduction was in the range of 10 to 50 μm. The value obtained by dividing the amount of thickness reduction (μm) by the spray time (min) was taken as the etching rate (μm / min) of the test material. For a thin plate material of a Cu-Ni-Al-based copper alloy, if the etching rate in this etching test is, for example, 12 μm / min or more, it can be evaluated that a significant improvement in the etching rate is observed compared to conventional ones. The test results are shown in Tables 5 and 6.
[0064] [Table 2]
[0065] [Table 3]
[0066] [Table 4]
[0067] [Table 5]
[0068] [Table 6]
[0069] The Cu-Ni-Al-based copper alloy sheets of the present invention all had an X-ray diffraction intensity ratio X A The values were high, and a significant improvement in the etching rate was observed compared to the comparative examples. The strength level was also high.
[0070] Comparative Example No. 31 is an example in which the tension was low in the solution treatment. No. 32 is an example in which the heating rate in the aging treatment was low. No. 33 is an example in which the tension in the final heat treatment was low. No. 34 is an example in which the final pass temperature in hot rolling was low, and further in which the tension in the solution treatment was low and the cooling rate was low. No. 40 is an example in which the holding time in the solution treatment was short and the heating rate in the aging treatment was low. No. 41 is an example in which the number of passes in the final cold rolling where the reduction ratio per pass was 12% or more was less than 4 passes. All of these have an X-ray diffraction intensity ratio X A The value was low, and the improvement in the etching rate was insufficient.
[0071] Comparative Example No. 35 is an example in which the Ni content was low. Comparative Example No. 39 is an example in which the Al content was low and the Ni / Al ratio was high. In these examples, despite the use of the appropriate manufacturing conditions specified in the present invention, a sufficiently high X-ray diffraction intensity ratio X A No value was obtained and the etch rate was low.
[0072] Comparative Example No. 36 is an example where the Al content was high. No. 37 is an example where the Ni content was high. No. 38 is an example where the slab heating temperature was too high. In these examples, cracks occurred in the material during hot rolling, so it was not possible to proceed to the subsequent process.
Claims
1. The alloy has a chemical composition, in mass%, of Ni: 10.0 to 30.0%, Al: 1.0 to 6.5%, Ag: 0 to 0.5%, B: 0 to 0.1%, Be: 0 to 0.15%, Co: 0 to 2.0%, Cr: 0 to 0.5%, Fe: 0 to 2.0%, Ga: 0 to 0.5%, Ge: 0 to 0.5%, In: 0 to 0.5%, Mg: 0 to 0.5%, Mn: 0 to 2.0%, P: 0 to 0.2%, Si: 0 to 0.8%, Sn: 0 to 2.0%, Ti: 0 to 2.0%, Zn: 0 to 2.0%, Zr: 0 to 0.3%, and the balance being Cu and unavoidable impurities, and satisfies the following formula (1), and in the X-ray diffraction pattern of the plate surface, the X of the following formula (2) is A The value is 1.5 x 10 -3 The copper alloy sheet material is as described above. Ni / Al≦9.0…(1) Here, the content value of the element expressed as mass % is substituted for the element symbol in formula (1). X A =I{110} / (I{111}+I{200}+I{220}+I{311}+I{331}+I{420}) …(2) Here, I{110} is Ni 3 The integrated intensity of the diffraction peak of the {110} crystal plane of the Al-type precipitate, and the other I{hkl} are the diffraction peaks of the {hkl} crystal plane of the parent phase and Ni 3 This is the integrated intensity of the diffraction peaks in which the diffraction peaks of the {hkl} crystal planes of the Al-type precipitates are superimposed.
2. In the X-ray diffraction pattern of the plate surface, X of the following formula (3) B The copper alloy sheet material according to claim 1, wherein the value is 0.20 or more. X B =I{220} / (I{111}+I{200}+I{220}+I{311}+I{331}+I{420}) …(3) Here, I{hkl} is the diffraction peak of the parent phase {hkl} crystal plane and Ni 3 This is the integrated intensity of the diffraction peaks in which the diffraction peaks of the {hkl} crystal planes of the Al-type precipitates are superimposed.
3. The number density of coarse precipitate particles with a major axis of 1 μm or more on an observation surface parallel to the plate surface is 3.0 × 10 4 pieces / mm 2 The copper alloy sheet material according to claim 1 or 2, wherein:
4. The number density of fine precipitate particles with a major axis of 5 to 50 nm in the observation plane parallel to the plate surface is 1.0 × 10 7 pieces / mm 2 The copper alloy sheet material according to any one of claims 1 to 3.
5. The copper alloy sheet material according to any one of claims 1 to 4, having a tensile strength in the rolling direction of 900 MPa or more.
6. The copper alloy sheet material according to any one of claims 1 to 5, having a sheet thickness of 0.02 to 0.40 mm.
7. A step of heating a slab having a chemical composition, in mass%, of Ni: 10.0 to 30.0%, Al: 1.0 to 6.5%, Ag: 0 to 0.5%, B: 0 to 0.1%, Be: 0 to 0.15%, Co: 0 to 2.0%, Cr: 0 to 0.5%, Fe: 0 to 2.0%, Ga: 0 to 0.5%, Ge: 0 to 0.5%, In: 0 to 0.5%, Mg: 0 to 0.5%, Mn: 0 to 2.0%, P: 0 to 0.2%, Si: 0 to 0.8%, Sn: 0 to 2.0%, Ti: 0 to 2.0%, Zn: 0 to 2.0%, Zr: 0 to 0.3%, with the balance being Cu and unavoidable impurities, and satisfying the following formula (1), at 1000 to 1150 ° C. (slab heating step); A process of performing hot rolling under conditions in which the rolling temperature in the final rolling pass is 800 ° C. or higher (hot rolling process); Cold rolling process (cold rolling process) 5 to 25 N / mm 2 a step of holding the steel sheet at 950 to 1100°C for 30 to 360 seconds while applying a tension of 100°C to the steel sheet, and then cooling the steel sheet at an average cooling rate of 80°C / s or more from 900°C to 300°C (solution treatment step); A process of increasing the temperature from 300° C. to 400° C. at an average heating rate of 40° C. / h or more and holding the temperature at 400 to 650° C. for 0.1 to 75 hours (aging treatment process); A process of performing cold rolling with a total rolling ratio of 40% or more in a pass schedule including four or more rolling passes with a rolling ratio of 12% or more per pass (final cold rolling process); 70-150N / mm 2 a step of holding the sheet at 400 to 700° C. for 10 to 600 seconds while applying a tension of In the above order, the manufacturing process includes the steps of: A The value is 1.5 x 10 -3 A method for producing a copper alloy sheet material, which obtains the above-mentioned sheet material. Ni / Al≦9.0…(1) Here, the content value of the element expressed as mass % is substituted for the element symbol in formula (1). X A =I{110} / (I{111}+I{200}+I{220}+I{311}+I{331}+I{420}) …(2) Here, I{110} is Ni 3 The integrated intensity of the diffraction peak of the {110} crystal plane of the Al-type precipitate, and the other I{hkl} are the diffraction peaks of the {hkl} crystal plane of the parent phase and Ni 3 This is the integrated intensity of the diffraction peaks in which the diffraction peaks of the {hkl} crystal planes of the Al-type precipitates are superimposed.
8. X in the formula (2) A The value is 1.5 x 10 -3 or more, and X in the following formula (3) B The method for producing a copper alloy sheet according to claim 7, wherein a sheet having a value of 0.20 or more is obtained. X B =I{220} / (I{111}+I{200}+I{220}+I{311}+I{331}+I{420}) …(3) Here, I{hkl} is the diffraction peak of the parent phase {hkl} crystal plane and Ni 3 This is the integrated intensity of the diffraction peaks in which the diffraction peaks of the {hkl} crystal planes of the Al-type precipitates are superimposed.
9. The method for producing a copper alloy sheet according to claim 7 or 8, wherein a sheet having a thickness of 0.02 to 0.40 mm is obtained in the final cold rolling step.
10. A conductive spring member using the copper alloy sheet material according to any one of claims 1 to 6 as a material.
Citation Information
Patent Citations
Copper base alloy for connector and its production
JP1993320790A
Cu-Ni-Al-BASED COPPER ALLOY SHEET MATERIAL, MANUFACTURING METHOD THEREOF, AND CONDUCTIVE SPRING MEMBER
JP2019002042A
Cu-Ni-Al-BASED COPPER ALLOY SHEET MATERIAL, MANUFACTURING METHOD THEREFOR, AND CONDUCTIVE SPRING MEMBER
JP2020050923A
HIGH YOUNG Cu-Ni-Al-BASED COPPER ALLOY SHEET, METHOD FOR PRODUCING THE SAME, AND CONDUCTIVE SPRING MEMBER