Adhesive composition for polarizing plate, polarizing plate and optical display device

The adhesive composition for polarizing plates, composed of polyvinyl alcohol resin, crosslinking agents, and epoxy compounds, addresses the limitations of photocurable adhesives by providing strong, durable, and flexible bonding between polarizers and liquid crystal retardation layers, enhancing the performance of light emitting displays.

JP7595158B2Active Publication Date: 2024-12-05ホアードサン ヘンシン(ウーシー) マテリアルズ カンパニーリミテッド
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2023522906
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-10-27
Filing Date
2021-10-26
Publication Date
2024-12-05
Estimated Expiration
2041-10-26

AI Technical Summary

Technical Problem

Existing adhesive layers used in polarizing plates for light emitting displays, particularly those formed from photocurable adhesives, face limitations in thickness reduction and adhesive strength, especially when bonding liquid crystal films with low adhesiveness, leading to issues with bending reliability and high-temperature, high-humidity durability.

Method used

An adhesive composition comprising polyvinyl alcohol resin, a crosslinking agent with primary or secondary amine groups, and an epoxy compound with an alkylene oxide group is used to form adhesive layers with enhanced strength and durability, allowing for thinner layers and improved bonding between polarizers and liquid crystal retardation layers.

Benefits of technology

The adhesive composition achieves excellent adhesive strength, high-temperature, high-humidity durability, and bending reliability, enabling successful bonding of polarizers and liquid crystal retardation layers, even when the latter have low adhesiveness, and facilitates the production of thinner polarizing plates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007595158000005
    Figure 0007595158000005
  • Figure 0007595158000006
    Figure 0007595158000006
  • Figure 0007595158000007
    Figure 0007595158000007
Patent Text Reader

Abstract

Provided are an adhesive composition for polarizing plates, a polarizing plate, and an optical display device, which comprise a polyvinyl alcohol resin, a crosslinking agent having a primary amine group or a secondary amine group, and an epoxy compound having an alkylene oxide group.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an adhesive composition for polarizing plates, a polarizing plate, and an optical display device. [Background technology]

[0002] Light emitting display devices including organic light emitting display devices may not include a polarizing plate. However, incident external light may be totally reflected by a panel in the light emitting display device, thereby degrading the quality of the screen. For this reason, light emitting display devices generally include a polarizing plate on the upper surface of the panel. The polarizing plate is composed of a polarizer and a retardation film. The retardation film may be a polymer film, but due to the recent trend toward thinner displays, a liquid crystal film is used.

[0003] When bonding a polarizer and a liquid crystal film, it is common to use a pressure-sensitive adhesive layer between the polarizer and the liquid crystal film, and between the two liquid crystal films, especially when two liquid crystal films are used. However, the pressure-sensitive adhesive layer has a disadvantage in terms of bending reliability required for flexible displays. Therefore, a method of using an adhesive layer made of a photocurable adhesive instead of the pressure-sensitive adhesive layer is being considered.

[0004] However, the adhesive layer formed with a photocurable adhesive has limitations in terms of how thin it can be made compared to a water-based adhesive, and yet when a liquid crystal film is bonded with a water-based adhesive, it is difficult to bond a polarizer and a liquid crystal film, or a liquid crystal film and another liquid crystal film, with high adhesive strength, because the liquid crystal film is a non-adhesive film with low adhesiveness.

[0005] The background art of the present invention is disclosed in Korean Patent Publication No. 10-2006-0103451 and the like. Summary of the Invention [Problem to be solved by the invention]

[0006] An object of the present invention is to provide an adhesive composition for polarizing plates that forms an adhesive layer having excellent adhesive strength between a polarizer and a liquid crystal retardation layer and between liquid crystal retardation layers.

[0007] Another object of the present invention is to provide an adhesive composition for polarizing plates that forms an adhesive layer having excellent adhesive strength between a liquid crystal retardation layer having low adhesiveness and a polarizer, and excellent adhesive strength between each liquid crystal retardation layer having low adhesiveness.

[0008] It is still another object of the present invention to provide an adhesive composition for polarizing plates which forms an adhesive layer excellent in high-temperature and high-humidity durability and bending reliability.

[0009] It is still another object of the present invention to provide a polarizing plate and an optical display device which include the above-mentioned adhesive layer. [Means for solving the problem]

[0010] One aspect of the present invention is an adhesive composition for polarizing plates.

[0011] 1. The adhesive composition for polarizing plates comprises a polyvinyl alcohol resin; a crosslinking agent having a primary amine group (-NH2) or a secondary amine group (-NH-); and an epoxy compound having an alkylene oxide group.

[0012] In 2.1, the crosslinking agent having a primary amine group or a secondary amine group may include one or more ethyleneimine-based crosslinking agents.

[0013] In 3.1 to 2, the crosslinking agent and the epoxy compound having an alkylene oxide group may be contained in a weight ratio of 1:1 to 1:15.

[0014] In 4.1 to 3, the alkylene oxide group may be *-[-OR-]-* (* is a linking moiety, and R is a linear or branched alkylene group having 2 to 4 carbon atoms).

[0015] In 5.1 to 5.4, the epoxy compound having an alkylene oxide group may include a compound represented by the following formula 1:

[0016] [ka]

[0017] (In the above Chemical Formula 1, R is a linear or branched alkylene group having 2 to 4 carbon atoms; R 1 , R 2 each independently represents an epoxide group or an epoxide group-containing group, n is an integer from 1 to 30. In 6.1 to 5, the epoxy compound having an alkylene oxide group can include one or more of ethylene glycol diglycidyl ether; poly(ethylene glycol) diglycidyl ether; propylene glycol diglycidyl ether; and poly(propylene glycol) diglycidyl ether.

[0018] In 7.1 to 6, the composition may include 100 parts by weight of the polyvinyl alcohol resin, about 0.1 to about 50 parts by weight of the crosslinking agent having a primary amine group or a secondary amine group, and about 1 to about 100 parts by weight of the epoxy compound having an alkylene oxide group.

[0019] Another aspect of the present invention is a polarizing plate.

[0020] 8. A polarizing plate includes a polarizer, a first liquid crystal retardation layer laminated on a lower surface of the polarizer, and a first adhesive layer that bonds the polarizer and the first liquid crystal retardation layer, and the first adhesive layer includes an adhesive layer formed from the adhesive composition for polarizing plates of the present invention.

[0021] In 9.8, the first liquid crystal retardation layer can contain an aromatic ring-containing liquid crystal compound.

[0022] In 10.8 to 9, a second adhesive layer and a second liquid crystal retardation layer may be further laminated on the lower surface of the first liquid crystal retardation layer.

[0023] In 11.8 to 10, the second liquid crystal retardation layer may contain an aromatic ring-containing liquid crystal compound.

[0024] In 12.8 to 11, the second adhesive layer may be formed of an adhesive composition for polarizing plates, which includes a polyvinyl alcohol resin, a crosslinking agent having a primary amine group or a secondary amine group, and an epoxy compound having an alkylene oxide group.

[0025] In 13.12, the crosslinking agent having a primary amine group or a secondary amine group may include one or more ethyleneimine-based crosslinking agents.

[0026] 14. In 12 to 13, the epoxy compound having an alkylene oxide group can include one or more of ethylene glycol diglycidyl ether; poly(ethylene glycol) diglycidyl ether; propylene glycol diglycidyl ether; and poly(propylene glycol) diglycidyl ether.

[0027] Yet another aspect of the present invention is an optical display device.

[0028] The optical display device comprises the polarizing plate of the present invention. Effect of the Invention

[0029] The present invention can provide an adhesive composition for polarizing plates that forms an adhesive layer having excellent adhesive strength between a polarizer and a liquid crystal retardation layer and between liquid crystal retardation layers.

[0030] The present invention can provide an adhesive composition for polarizing plates that forms an adhesive layer having excellent adhesive strength between a liquid crystal retardation layer having low adhesiveness and a polarizer, and excellent adhesive strength between each liquid crystal retardation layer having low adhesiveness.

[0031] The present invention can provide an adhesive composition for polarizing plates that forms an adhesive layer excellent in high-temperature and high-humidity durability and bending reliability.

[0032] The present invention can provide a polarizing plate and an optical display device including the above-mentioned adhesive layer. [Brief description of the drawings]

[0033] [Figure 1] FIG. 2 is a cross-sectional view of a polarizing plate according to an embodiment of the present invention. [Diagram 2] FIG. 4 is a cross-sectional view of a polarizing plate according to another embodiment of the present invention. [Diagram 3] FIG. 2 is a schematic plan view of a test piece used in evaluating high-temperature and high-humidity durability. [Figure 4] FIG. 1 is a cross-sectional view of a test piece for bending reliability evaluation. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0034] [Best Mode for Carrying Out the Invention] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will now be described in detail with reference to the accompanying drawings, in which: FIG.

[0035] In the drawings, in order to clearly explain the present invention, parts that are not related to the description are omitted, and the same names are used for the same or similar components throughout the specification. In the drawings, the length and size of each component are for explaining the present invention, and the present invention is not limited to the length and size of each component illustrated in the drawings.

[0036] In this specification, "upper" and "lower" are defined with reference to the drawings, and "upper" may be changed to "lower" and "lower" to "upper" depending on the viewpoint, and "on" may include not only directly on but also cases where another structure is interposed between them. Meanwhile, "directly on", "directly on" or "directly formed" indicates that no other structure such as an intermediate body is interposed between them.

[0037] In this specification, when describing a numerical range, "X to Y" means "X or more, Y or less" (X≦and≦Y).

[0038] The adhesive composition for polarizing plate of the present invention formed an adhesive layer having excellent adhesion to the adherend, which is the liquid crystal retardation layer described in detail below. The adhesive composition for polarizing plate of the present invention formed an adhesive layer having excellent adhesion between the polarizer and the liquid crystal retardation layer, and formed an adhesive layer having excellent adhesion between the liquid crystal retardation layer and the liquid crystal retardation layer. In general, the liquid crystal retardation layer is attached to the polarizer in the form of a liquid crystal retardation film including a substrate film and a liquid crystal retardation layer formed on the upper surface of the substrate film, and then the substrate film is removed from the liquid crystal retardation layer to be included in the polarizing plate. If the adhesive strength between the liquid crystal retardation layer and the polarizer is low, the liquid crystal retardation layer is peeled off from the polarizer during the process of peeling off the substrate film, making it difficult to manufacture the polarizing plate.

[0039] In addition, the adhesive composition for polarizing plates of the present invention formed an adhesive layer having excellent high-temperature and high-humidity durability and bending reliability. The polarizing plate of the present invention included an adhesive layer formed from the above-mentioned adhesive composition for polarizing plates, and had excellent high-temperature and high-humidity durability and bending reliability.

[0040] Hereinafter, a polarizing plate according to an embodiment of the present invention will be described with reference to FIG.

[0041] 1, the polarizing plate includes a polarizer 100, a first adhesive layer 300, a first liquid crystal retardation layer 200, and a third protective layer 400. The third protective layer 400 is laminated on an upper surface of the polarizer 100, and the polarizer 100, the first adhesive layer 300, and the first liquid crystal retardation layer 200 are sequentially laminated on a lower surface of the polarizer 100.

[0042] Polarizer The polarizer 100 may include a conventional polarizer known to those skilled in the art. For example, the polarizer may include a polarizer manufactured from a polyvinyl alcohol (PVA)-based resin film or a polypropylene (PP)-based resin film. Specifically, the polarizer may be a polyvinyl alcohol-based polarizer in which one or more of iodine and a heterochromatic dye are adsorbed to a polyvinyl alcohol-based resin film, or a polyene-based polarizer manufactured by dehydrating a polyvinyl alcohol-based resin film. The saponification degree of the polyvinyl alcohol-based resin film may be about 85 mol% to about 100 mol%, specifically about 98 mol% to about 100 mol%. The polymerization degree of the polyvinyl alcohol-based resin film may be about 1,000 to about 10,000, specifically about 1,500 to about 10,000. A polarizer having the above saponification degree and polymerization degree may be manufactured. The polarizer may be manufactured by a conventional method known to those skilled in the art.

[0043] The thickness of the polarizer 100 may be about 5 μm to about 30 μm, specifically about 5 μm to about 25 μm. In this range, the polarizer 100 can be used as a polarizing plate, and the effect of making the polarizing plate thinner can be realized.

[0044] 1st liquid crystal retardation layer The first liquid crystal retardation layer 200 converts the linearly polarized light emitted after the external light passes through the polarizer 100 into circularly polarized light, thereby preventing reflection of the external light and improving the screen quality.

[0045] In one embodiment, the first liquid crystal retardation layer 200 has an in-plane retardation (Re) of about 100 nm to about 220 nm, specifically about 100 nm to about 180 nm, for example, λ / 4 retardation, at a wavelength of 550 nm. In this range, the reflectance of external light can be reduced, and the image quality can be improved.

[0046] In another embodiment, the first liquid crystal retardation layer 200 has an in-plane retardation (Re) of about 225 nm to about 350 nm, specifically about 225 nm to about 300 nm, for example, λ / 2 retardation, at a wavelength of 550 nm. In this range, the reflectance of external light can be reduced, and the image quality can be improved.

[0047] In this specification, the "in-plane retardation (Re)" can be calculated by Re = (nx - ny) × d (nx and ny are the refractive indices in the slow axis direction and the fast axis direction of the liquid crystal retardation layer, respectively, and d is the thickness (unit: nm) of the liquid crystal retardation layer).

[0048] The thickness of the first liquid crystal retardation layer 200 may be about 0.1 μm to about 30 μm, for example, about 1 μm to about 10 μm. In this range, the polarizer can be thinned and a desired retardation can be realized.

[0049] The first liquid crystal retardation layer 200 has low adhesion. The low adhesion may be caused by the first liquid crystal retardation layer being made of a liquid crystal composition.

[0050] In one embodiment, the first liquid crystal retardation layer 200 may contain a hydrophobic aromatic ring-containing liquid crystal compound. The first liquid crystal retardation layer is formed by coating a liquid crystal retardation layer composition on a substrate film and curing the composition, and the aromatic ring-containing liquid crystal compound may be oriented to realize the above-mentioned in-plane retardation. The aromatic ring-containing liquid crystal compound may be mechanically oriented, physically oriented, or optically oriented on the substrate film. The substrate film may not have an orientation film formed on one side, and may further have an orientation film formed on one side to make it easier to align the aromatic ring-containing liquid crystal compound. The substrate film is an optically transparent resin film, and the type thereof is not particularly limited. For example, the substrate film may be a cellulose-based resin film such as triacetyl cellulose (TAC), but is not limited thereto.

[0051] In one embodiment, the aromatic ring-containing liquid crystal compound may be a polymer, oligomer, or monomer that includes a unit composed of an aromatic ring and a polymerizable functional group that can impart liquid crystallinity. The polymerizable functional group may be a (meth)acryloyl group, an epoxy group, a vinyl ether group, or the like, and may be cured by heat or light to increase the strength of the first liquid crystal retardation layer.

[0052] The first liquid crystal retardation layer may be formed of a composition containing the above-mentioned aromatic ring-containing liquid crystal compound. The composition may further contain additives such as a leveling agent, a polymerization initiator, an alignment assistant, a heat stabilizer, a lubricant, a plasticizer, and an antistatic agent, and the detailed types of these are known to those skilled in the art.

[0053] Although not shown in Fig. 1, an adhesive layer or a bonding layer is formed on the lower surface of the first liquid crystal retardation layer 200, so that the polarizing plate can be attached to an optical display panel, etc. The adhesive layer or the bonding layer may be formed of a (meth)acrylic composition known to those skilled in the art, but is not limited thereto.

[0054] 1st adhesive layer The first adhesive layer 300 is formed between the polarizer 100 and the first liquid crystal retardation layer 200, and can adhere the polarizer 100 and the first liquid crystal retardation layer 200 to each other.

[0055] In a specific example, the first adhesive layer 300 may be directly formed on the polarizer 100 and the first liquid crystal retardation layer 200. The term "directly formed" means that no adhesive layer, adhesive layer or tacky adhesive layer other than the first adhesive layer 300 is formed between the polarizer 100 and the first liquid crystal retardation layer 200.

[0056] The thickness of the first adhesive layer 300 may be about 10 nm to about 500 nm, for example, about 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm, 100 nm, 110 nm, 120 nm, 130 nm, 140 nm, 150 nm, 160 nm, 170 nm, 180 nm, 190 nm, 200 nm, 210 nm, 220 nm, 230 nm, 240 nm, 250 nm, 260 nm, 270 nm, 280 nm, 290 nm, 300 nm, 310 nm, 320 nm, 330 nm, 340 nm, 350 nm, 360 nm, 370 nm, 380 nm, 390 nm, 400 nm, 410 nm, 420 nm, 430 nm, 440 nm, 450 nm, 460 nm, 470 nm, 480 nm, 490 nm, 500 nm, 510 nm, 520 nm, 530 nm, 540 nm, 550 nm, 560 nm, 570 nm, 580 nm, 590 nm, 600 nm, 610 nm, 620 nm, 630 nm, 640 nm, 650 nm, 660 nm, 670 nm, 680 nm, 690 nm, 700 nm, 710 nm, 720 nm, 730 nm, 740 nm, 750 nm, 760 nm, 770 nm, 780 nm, 790 nm, 800 nm, 810 nm, 820 60nm, 270nm, 280nm, 290nm, 300nm, 310nm, 320nm, 330nm, 340nm, 350nm, 360nm, 370nm, 380nm, 390nm, 400nm, 410nm, 420nm, 430nm, 440nm, 450nm, 460nm, 470nm, 480nm, 490nm, 500nm, specifically, about 50nm to about 200nm. Within this range, the effect of making the polarizing plate thinner can be obtained.

[0057] The first adhesive layer 300 is formed of an adhesive composition for a polarizing plate, which will be described in detail below, and thus provides a polarizing plate having excellent adhesion to the polarizer 100 and the first liquid crystal retardation layer 200, durability at high temperature and high humidity, and bending reliability at high temperature and high humidity. The adhesive composition for a polarizing plate will be described in detail below.

[0058] The adhesive composition for polarizing plates includes a polyvinyl alcohol resin, a crosslinking agent having a primary amine group (-NH2) or a secondary amine group (-NH-), and an epoxy compound having an alkylene oxide group. Through this, the adhesive composition for polarizing plates realizes the above-mentioned effects of the adhesive layer. In addition, the adhesive composition for polarizing plates is a water-based adhesive composition, and can form a thinner adhesive layer than a photocurable adhesive composition.

[0059] The adhesive composition for polarizing plates is a thermosetting composition, and can form an adhesive layer by thermal curing.

[0060] The adhesive composition for polarizing plates may further contain an aqueous solvent. The aqueous solvent makes it easy to apply the adhesive composition and enables the formation of a thin adhesive layer.

[0061] The aqueous solvent may be water, including ultrapure water, but is not limited thereto. The aqueous solvent may be contained in the adhesive composition in the remaining amount.

[0062] The polyvinyl alcohol-based resin is a vinyl-based polymer, and when a polyvinyl alcohol-based polarizer is used as a polarizer, the polyvinyl alcohol-based resin may have superior adhesive strength to other adhesive resins.

[0063] The polyvinyl alcohol resin may include polyvinyl alcohol or its derivative obtained by saponifying polyvinyl acetate, or a saponified copolymer of vinyl acetate and a copolymerizable monomer, or a modified polyvinyl alcohol resin obtained by acetylating, urethane-forming, etherifying, grafting, or phosphorylating polyvinyl alcohol. These may be included alone or in a mixture of two or more. Examples of the copolymerizable monomer include unsaturated carboxylic acids or esters thereof such as (anhydrous) maleic acid, fumaric acid, crotonic acid, itaconic acid, and (meth)acrylic acid, α-olefins such as ethylene and propylene, (meth)allylsulfonic acid, monoalkyl maleates, disulfonic acid soda alkyl maleates, N-methylol acrylamide, alkali salts of acrylamido alkyl sulfonic acids, N-vinyl pyrrolidone, and N-vinyl pyrrolidone derivatives.

[0064] In one embodiment, the polyvinyl alcohol resin can include a polyvinyl alcohol resin containing an acetoacetyl group, which can help improve the water resistance of the adhesive layer.

[0065] In one embodiment, the degree of modification of the acetoacetyl group of the polyvinyl alcohol resin may be about 1 mol% to about 30 mol%, for example, 1 mol%, 5 mol%, 10 mol%, 15 mol%, 20 mol%, 25 mol%, 30 mol%, specifically about 1 mol% to about 10 mol%. In the above range, sufficient reaction points with the crosslinking agent can be provided to exhibit adhesive strength and improve the water resistance of the polarizing plate. The method of preparing the polyvinyl alcohol resin containing the acetoacetyl group is not particularly limited. For example, a method of dispersing the polyvinyl alcohol resin in acetic acid and adding diketene can be considered, but is not limited thereto.

[0066] The average polymerization degree and saponification degree of the polyvinyl alcohol resin are not particularly limited, but the average polymerization degree is about 100 to about 3000, for example, 100, 500, 1000, 1500, 2000, 2500, 3000, and the average saponification degree is about 85 mol% to about 100 mol%, for example, 85 mol%, 86 mol%, 87 mol%, 88 mol%, 89 mol%, 90 mol%, 91 mol%, 92 mol%, 93 mol%, 94 mol%, 95 mol%, 96 mol%, 97 mol%, 98 mol%, 99 mol%, 100 mol%. In the above range, the adhesive strength between the polarizer and the first liquid crystal retardation layer may be further improved.

[0067] The polyvinyl alcohol-based resin may be included in an amount of about 1 part by weight to about 20 parts by weight, for example, about 1 part by weight, 2 parts by weight, 3 parts by weight, 4 parts by weight, 5 parts by weight, 6 parts by weight, 7 parts by weight, 8 parts by weight, 9 parts by weight, 10 parts by weight, 11 parts by weight, 12 parts by weight, 13 parts by weight, 14 parts by weight, 15 parts by weight, 16 parts by weight, 17 parts by weight, 18 parts by weight, 19 parts by weight, 20 parts by weight, specifically about 1 part by weight to about 10 parts by weight, based on 100 parts by weight of the aqueous solvent. In this range, the adhesive strength of the adhesive layer can be exhibited, and the viscosity of the adhesive composition does not increase rapidly, so that the processability can be excellent.

[0068] The crosslinking agent having the primary amine group (-NH2) and / or secondary amine group (-NH-) can provide adhesive strength to the adhesive layer by reacting with the polyvinyl alcohol resin and the epoxy compound having an alkylene oxide group described in detail below.

[0069] The crosslinking agent is linear, branched or dendrimer type and has a plurality of primary amine groups (-NH2) or secondary amine groups (-NH-), so that it can provide adhesive strength to the adhesive layer. In addition, the crosslinking agent was selected from among a plurality of crosslinking agents used in water-based adhesives for polarizing plates, because it reacts with an epoxy-based compound described in detail below and provides all of adhesive strength, high temperature and high humidity durability and bending reliability.

[0070] In one embodiment, the crosslinking agent having a primary amine group or a secondary amine group may include one or more ethyleneimine-based crosslinking agents. The "ethyleneimine-based crosslinking agent" may include a crosslinking agent synthesized by treating ethyleneimine with one or more of ring opening, polymerization, derivatization, etc., according to a known method. Specifically, the ethyleneimine-based crosslinking agent may include a poly(ethyleneimine)-based crosslinking agent.

[0071] The poly(ethyleneimine)-based crosslinking agent may include a linear, branched, or dendrimer-type compound having a primary amine group and / or a secondary amine group at the end and a secondary amine group and / or a tertiary amine group in the main chain. The primary amine group and / or the secondary amine group can increase the adhesive strength by reacting with the functional group of the polyvinyl alcohol-based resin, specifically, the hydroxyl group or the acetoacetyl group.

[0072] As known to those skilled in the art, poly(ethyleneimine)-based crosslinkers may include crosslinkers in which an ethylene group (-CHCH-) is linked to a secondary amine group and / or a tertiary amine group and has a primary amine group and / or a secondary amine group at its terminal.

[0073] The weight average molecular weight of the crosslinking agent is not particularly limited, but may be about 100 to about 1,000,000. Within this range, the adhesive layer of the present invention can exhibit its effect.

[0074] The crosslinking agent is used in an amount of about 0.1 to about 50 parts by weight, for example, about 0.1 parts by weight, 0.5 parts by weight, 1 parts by weight, 1.5 parts by weight, 2 parts by weight, 2.5 parts by weight, 3 parts by weight, 3.5 parts by weight, 4 parts by weight, 4.5 parts by weight, 5 parts by weight, 5.5 parts by weight, 6 parts by weight, 6.5 parts by weight, 7 parts by weight, 7.5 parts by weight, 8 parts by weight, 8.5 parts by weight, 9 parts by weight, 9.5 parts by weight, 10 parts by weight, 11 parts by weight, 12 parts by weight, 13 parts by weight, 14 parts by weight, 15 parts by weight, 16 parts by weight, 17 parts by weight, 18 parts by weight, 19 parts by weight, 20 parts by weight, 21 parts by weight, 22 parts by weight, 23 parts by weight, 24 parts by weight, 25 parts by weight, 26 parts by weight, 27 parts by weight, 28 parts by weight, 29 parts by weight, 30 parts by weight, 31 parts by weight, 32 parts by weight, 33 parts by weight, 34 parts by weight, 35 parts by weight, 36 parts by weight, 37 parts by weight, 38 parts by weight, 39 parts by weight, 40 parts by weight, 41 parts by weight, 42 parts by weight, 43 parts by weight, 44 parts by weight, 45 parts by weight, 46 parts by weight, 47 parts by weight, 48 parts by weight, 49 parts by weight, 50 parts by weight, 51 parts by weight, 52 parts by weight, 53 parts by weight, 54 parts by weight, 55 parts by weight, 56 parts by weight, 57 parts by weight, 58 parts Parts by weight, 22 parts by weight, 23 parts by weight, 24 parts by weight, 25 parts by weight, 26 parts by weight, 27 parts by weight, 28 parts by weight, 29 parts by weight, 30 parts by weight, 31 parts by weight, 32 parts by weight, 33 parts by weight, 34 parts by weight, 35 parts by weight, 36 parts by weight, 37 parts by weight, 38 parts by weight, 39 parts by weight, 40 parts by weight, 41 parts by weight, 42 parts by weight, 43 parts by weight, 44 parts by weight, 45 parts by weight, 46 parts by weight, 47 parts by weight, 48 parts by weight, 49 parts by weight, 50 parts by weight, specifically about 0.5 parts by weight to about 10 parts by weight, more specifically about 1 part by weight to about 10 parts by weight, about 1 part by weight to about 5 parts by weight. In the above range, the adhesive strength of the adhesive layer may be good.

[0075] The crosslinker:epoxy compound having an alkylene oxide group may be included in the adhesive composition in a weight ratio of about 1:1 to about 1:15, for example, about 1:1, 1:2, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9, 1:10, 1:11, 1:12, 1:13, 1:14, 1:15, specifically about 1:1 to about 1:10, more specifically about 1:1 to about 1:5. Within this range, the epoxy group of the epoxy compound and the amine group of the crosslinker may sufficiently react to improve the cohesive strength inside the adhesive, thereby improving the adhesive strength.

[0076] Meanwhile, the first liquid crystal retardation layer may have a problem that the aqueous adhesive is not applied well because it is formed of the hydrophobic aromatic ring liquid crystal compound described above. However, an epoxy-based compound having an alkylene oxide group can solve the above problem. In one embodiment, the epoxy-based compound having an alkylene oxide may be a non-aromatic compound having no aromatic group. In addition, the epoxy-based compound reacts with the crosslinking agent through the epoxy group, and the crosslinking agent reacts with the polyvinyl alcohol resin, thereby finally providing an adhesive layer having high adhesive strength.

[0077] In addition, the epoxy compound having an alkylene oxide group enables the adhesive composition to be smoothly applied to the liquid crystal retardation layer with a predetermined thickness when the adhesive composition is applied to the liquid crystal retardation layer, thereby enabling the formation of a uniform adhesive layer.

[0078] The alkylene oxide group-containing epoxy compound may include a linear or branched compound having an alkylene oxide group repeat unit in the compound molecule and an epoxy group at a side chain and / or terminal.

[0079] The "alkylene oxide group" may be *-[-OR-]-* (* is a linking moiety, and R is a linear or branched alkylene group having 2 to 4 carbon atoms). For example, the alkylene oxide group may be an ethylene oxide group, an n-propylene oxide group, or an iso-propylene oxide group. The "epoxy group" may be an epoxide group or a glycidoxy group. In one embodiment, the epoxy compound having an alkylene oxide group may include, but is not limited to, a compound represented by the following Chemical Formula 1:

[0080] [ka]

[0081] (In the above Chemical Formula 1, R is a linear or branched alkylene group having 2 to 4 carbon atoms; R 1 , R 2 each independently represents an epoxide group or an epoxide group-containing group, n is an integer from 1 to 30. The epoxide group-containing group may be a glycidyl group or a glycidoxy group.

[0082] n can be 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30.

[0083] For example, the epoxy compound having an alkylene oxide group may include one of monoalkylene glycol diglycidyl ether, polyalkylene glycol diglycidyl ether, monoalkylene glycol triglycidyl ether, and polyalkylene glycol diglycidyl ether, for example, one or more of ethylene glycol diglycidyl ether; poly(ethylene glycol) diglycidyl ether including di(ethylene glycol) diglycidyl ether, tri(ethylene glycol) diglycidyl ether, etc.; propylene glycol diglycidyl ether; and poly(propylene glycol) diglycidyl ether, but is not limited thereto.

[0084] Preferably, the epoxy compound having an alkylene oxide group may include at least one of poly(ethylene glycol) diglycidyl ether and poly(propylene glycol) diglycidyl ether, which can improve bending reliability even at a smaller radius of curvature.

[0085] The epoxy compound having an alkylene oxide group is used in an amount of about 1 part by weight to about 100 parts by weight, for example, about 1 part by weight, 2 parts by weight, 3 parts by weight, 4 parts by weight, 5 parts by weight, 6 parts by weight, 7 parts by weight, 8 parts by weight, 9 parts by weight, 10 parts by weight, 11 parts by weight, 12 parts by weight, 13 parts by weight, 14 parts by weight, 15 parts by weight, 16 parts by weight, 17 parts by weight, 18 parts by weight, 19 parts by weight, 20 parts by weight, 21 parts by weight, 22 parts by weight, 23 parts by weight, 24 parts by weight, 25 parts by weight, 26 parts by weight, or the like, based on 100 parts by weight of the polyvinyl alcohol resin. Parts by weight, 27 parts by weight, 28 parts by weight, 29 parts by weight, 30 parts by weight, 31 parts by weight, 32 parts by weight, 33 parts by weight, 34 parts by weight, 35 parts by weight, 36 parts by weight, 37 parts by weight, 38 parts by weight, 39 parts by weight, 40 parts by weight, 45 parts by weight, 50 parts by weight, 55 parts by weight, 60 parts by weight, 65 parts by weight, 70 parts by weight, 75 parts by weight, 80 parts by weight, 85 parts by weight, 90 parts by weight, 95 parts by weight, 100 parts by weight, specifically about 1 part by weight to about 50 parts by weight, more specifically about 3 parts by weight to about 35 parts by weight. In this range, the adhesive strength of the adhesive layer may be good.

[0086] The adhesive composition for polarizing plates may further include common additives other than the above-mentioned polyvinyl alcohol resin, epoxy compound having an alkylene oxide group, and crosslinking agent having a primary amine group or a secondary amine group. For example, the additives may include one or more of a UV absorber, a heat stabilizer, a plasticizer, a surfactant, a reaction inhibitor, an adhesion improver, a thixotropy imparting agent, a conductivity imparting agent, an antioxidant, a leveling agent, and a stabilizer, but are not limited thereto.

[0087] 3rd protective layer The third protective layer 400 is formed on the upper surface of the polarizer 100 to protect the polarizer 100 and provide an additional function to the polarizing plate.

[0088] The third protective layer 400 may be an optically transparent protective film or protective coating layer, and may include any of those known to those skilled in the art. For example, the protective film may include one or more of cellulose ester-based resins including triacetyl cellulose (TAC) and the like, cyclic polyolefin-based resins including amorphous cyclic polyolefin and the like, polycarbonate-based resins, polyester-based resins including polyethylene terephthalate (PET) and the like, polyethersulfone-based resins, polysulfone-based resins, polyamide-based resins, polyimide-based resins, acyclic polyolefin-based resins, polyacrylate-based resins including polymethyl methacrylate resin and the like, polyvinyl alcohol-based resins, polyvinyl chloride-based resins, and polyvinylidene chloride-based resins.

[0089] The thickness of the third protective layer 400 is about 5 μm to about 200 μm, specifically about 30 μm to about 120 μm, and may be about 10 μm to about 100 μm in the case of a protective film type, and about 1 μm to about 50 μm in the case of a protective coating layer type. Within this range, the third protective layer 400 can be used in a polarizing plate.

[0090] Although not shown in FIG. 1, a functional coating layer such as a hard coating layer, an anti-fingerprint layer, an anti-reflection layer, etc. may be further formed on the upper surface of the third protective layer 400 to provide additional functions to the polarizer.

[0091] 1, the third protective layer 400 may be attached to the polarizer 100 by an adhesive layer. In this case, the adhesive layer may be formed of the above-mentioned adhesive composition for polarizing plates of the present invention, or may be formed of a water-based adhesive or a photocurable adhesive known to those skilled in the art.

[0092] Hereinafter, a polarizing plate according to another embodiment of the present invention will be described with reference to FIG.

[0093] 2, the polarizing plate includes a third protective layer 400, a polarizer 100, a first adhesive layer 300, a first liquid crystal retardation layer 200, a second adhesive layer 600, and a second liquid crystal retardation layer 500. The third protective layer 400 is laminated on the upper surface of the polarizer 100, and the first adhesive layer 300, the first liquid crystal retardation layer 200, the second adhesive layer 600, and the second liquid crystal retardation layer 500 are sequentially laminated on the lower surface of the polarizer 100. It is substantially the same as the polarizing plate of FIG. 1, except that the second adhesive layer 600 and the second liquid crystal retardation layer 500 are further formed on the lower surface of the first liquid crystal retardation layer 200.

[0094] Second liquid crystal retardation layer The second liquid crystal retardation layer 500 can prevent reflection of external light and improve the screen quality by converting linearly polarized light emitted after passing through the polarizer 100 into circularly polarized light.

[0095] In one embodiment, the second liquid crystal retardation layer 500 has an in-plane retardation (Re) of about 225 nm to about 350 nm at a wavelength of 550 nm, specifically about 225 nm to about 300 nm, for example, a λ / 2 retardation. In this range, the reflectance to external light can be reduced, and the image quality can be improved.

[0096] In another embodiment, the second liquid crystal retardation layer 500 has an in-plane retardation (Re) of about 100 nm to about 220 nm, specifically about 100 nm to about 180 nm, for example, λ / 4 retardation, at a wavelength of 550 nm. In this range, the reflectance of external light can be reduced, and the image quality can be improved.

[0097] The second liquid crystal retardation layer 500 may have a thickness of about 0.1 μm to about 30 μm, for example, about 1 μm to about 10 μm. In this range, the polarizer can be thinned to realize a desired retardation.

[0098] The second liquid crystal retardation layer 500 has low adhesion. The low adhesion may be due to the fact that the second liquid crystal retardation layer is formed of a liquid crystal composition and has nx and ny in appropriate ranges to realize the above-mentioned in-plane retardation.

[0099] In one embodiment, the second liquid crystal retardation layer 500 may contain a hydrophobic aromatic ring-containing liquid crystal compound. For example, the second liquid crystal retardation layer 500 may be formed of the composition described in the first liquid crystal retardation layer 200 above.

[0100] 2nd adhesive layer The second adhesive layer 600 is formed between the first liquid crystal retardation layer 200 and the second liquid crystal retardation layer 500, and can adhere the first liquid crystal retardation layer 200 and the second liquid crystal retardation layer 500 to each other.

[0101] In one embodiment, the second adhesive layer 600 may be directly formed on each of the first liquid crystal retardation layer 200 and the second liquid crystal retardation layer 500. The term "directly formed" means that no adhesive layer, adhesive layer or tacky adhesive layer other than the second adhesive layer 600 is formed between the first liquid crystal retardation layer 200 and the second liquid crystal retardation layer 500.

[0102] The thickness of the second adhesive layer 600 may be from about 10 nm to about 500 nm, for example, about 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm, 100 nm, 110 nm, 120 nm, 130 nm, 140 nm, 150 nm, 160 nm, 170 nm, 180 nm, 190 nm, 200 nm, 210 nm, 220 nm, 230 nm, 240 nm, 250 nm, , 260 nm, 270 nm, 280 nm, 290 nm, 300 nm, 310 nm, 320 nm, 330 nm, 340 nm, 350 nm, 360 nm, 370 nm, 380 nm, 390 nm, 400 nm, 410 nm, 420 nm, 430 nm, 440 nm, 450 nm, 460 nm, 470 nm, 480 nm, 490 nm, 500 nm, or about 50 nm to about 100 nm. Within the above range, the effect of making the polarizing plate thinner can be obtained.

[0103] In one embodiment, the second adhesive layer 600 may be formed of the adhesive composition for a polarizing plate of the present invention described above in the first adhesive layer 300. As a result, the adhesive composition for a polarizing plate of the present invention can realize an adhesive layer having excellent adhesion between a liquid crystal retardation layer having a high water contact angle and a liquid crystal retardation layer having a high water contact angle, and an adhesive layer having excellent adhesion between a liquid crystal retardation layer having a low adhesion and a liquid crystal retardation layer having a low adhesion.

[0104] In another embodiment, the second adhesive layer 600 may be formed of a conventional light-curing adhesive known to those skilled in the art. The light-curing adhesive may include an epoxy-based compound or a (meth)acrylic-based compound, and a photoinitiator. The epoxy-based compound or the (meth)acrylic-based compound, and the photoinitiator may be selected from conventional types known to those skilled in the art.

[0105] Although not shown in Fig. 2, an adhesive layer or a bonding layer is also formed on the lower surface of the second liquid crystal retardation layer 500, so that the polarizing plate can be attached to an optical display panel, etc. The adhesive layer or the bonding layer may be formed of a (meth)acrylic composition known to those skilled in the art, but is not limited thereto.

[0106] The method for producing the polarizing plate of the present invention will be described below.

[0107] A method for producing a polarizing plate may include the steps of forming a coating layer by applying the adhesive composition for a polarizing plate of the present invention to one surface of a liquid crystal retardation layer, bonding the coating layer to a polarizer, and curing the adhesive composition for a polarizing plate to bond the polarizer and the liquid crystal retardation layer.

[0108] The method for producing a polarizing plate may include the steps of forming a coating layer by applying the adhesive composition for a polarizing plate of the present invention to one surface of a liquid crystal retardation layer, bonding the coating layer to the liquid crystal retardation layer, and curing the adhesive composition for a polarizing plate to bond the liquid crystal retardation layer to the liquid crystal retardation layer.

[0109] The coating may be performed by a conventional method known to those skilled in the art, including, but not limited to, a die coater, a bar coater, etc. The curing may include thermally curing the coating layer. The thermal curing is not particularly limited, and may be performed at about 40° C. to about 100° C. for about 1 minute to about 60 minutes, for example, one or more times.

[0110] The optical display device of the present invention includes the polarizing plate of the present invention.

[0111] For example, the optical display device may include, but is not limited to, a light emitting display device, such as an organic light emitting display device, a liquid crystal display device, etc. For example, the optical display device may include a flexible optical display device.

[0112] [Mode for carrying out the invention] The present invention will be described in more detail with reference to the following examples, although the following examples are provided for the purpose of facilitating understanding of the present invention and the scope of the present invention is not limited to the following examples.

[0113] A. Third protective layer: COP film (G+, Zeon, a hard coating layer is formed on the upper surface. Thickness: 28 μm) B. First liquid crystal retardation film: A liquid crystal retardation film (FUJIFILM Corporation, QLAA) in which a liquid crystal retardation layer (having a λ / 2 retardation at a wavelength of 550 nm) is formed on the lower surface of a base film (TAC film). C. Second liquid crystal retardation film: A liquid crystal retardation film (FUJIFILM Corporation, QLAB) in which a liquid crystal retardation layer (having a λ / 4 retardation at a wavelength of 550 nm) is formed on the upper surface of a base film (TAC film). Example 1 <Manufacture of Polarizer> A polyvinyl alcohol film (Mitsubishi Chemical Corporation, polymerization degree: 2800, thickness: 20 μm) was immersed in a 0.3% iodine aqueous solution and adhered. The film was stretched in the MD direction at a stretch ratio of 5.0 times. The stretched polyvinyl alcohol film was immersed in a 3% boric acid aqueous solution and a 2% potassium iodide aqueous solution for hue correction. The film was dried at 50° C. for 4 minutes to produce a polarizer (thickness: 7 μm).

[0114] <Production of Water-Based Adhesive Composition for Polarizing Plates> 3 parts by weight of polyvinyl alcohol-based resin was added to 100 parts by weight of water at 95°C and dissolved with stirring for 60 minutes. After the obtained solution was completely cooled to room temperature, 0.1 parts by weight of crosslinker and 0.1 parts by weight of epoxy-based compound were added in order and mixed together, followed by stirring with a magnetic stirrer to prepare an adhesive composition for polarizing plates.

[0115] The following Table 1 shows the content (unit: parts by weight) of crosslinker and epoxy compound based on the solid content for 3 parts by weight of polyvinyl alcohol resin. In the following Table 1, "-" indicates that the corresponding component is not included.

[0116] <Production of photocurable adhesive composition for polarizing plates> A photocurable adhesive composition for polarizing plates was prepared by mixing 80 parts by weight of epoxy compound 2021P (3,4-epoxycyclohexylmethyl 3,4-epoxycyclohexanecarboxylate, Daicel Corporation), 20 parts by weight of epoxy compound EX141 (phenyl glycidyl ether, Nagase ChemteX Corporation), and 5 parts by weight of cationic polymerization initiator CPI100P (San-Apro Ltd.).

[0117] <Manufacture of polarizing plates> The aqueous adhesive composition for polarizing plates prepared above was applied to a predetermined thickness on each of the upper and lower surfaces of the prepared polarizer.

[0118] The lower surface of the COP film was placed on the upper surface of the polarizer, and the film was treated in a drying oven at 50° C. for 1 minute and then in a drying oven at 85° C. for 3 minutes. The liquid crystal retardation layer side of the first film for liquid crystal retardation layer was placed on the lower surface of the polarizer, and the film was treated in a drying oven at 50° C. for 1 minute and then in a drying oven at 85° C. for 3 minutes to manufacture a laminate of a third protective layer / adhesive layer / polarizer / adhesive layer / liquid crystal retardation layer / TAC film.

[0119] The prepared photocurable adhesive composition for polarizing plate was applied to a predetermined thickness on the liquid crystal retardation layer side of the film for the second liquid crystal retardation layer to form an adhesive coating layer. After removing the TAC film from the film for the first liquid crystal retardation layer, the liquid crystal retardation layer of the film for the first liquid crystal retardation layer was placed on the adhesive coating layer, and a metal halide lamp was used to illuminate the substrate film side of the film for the second liquid crystal retardation layer with an output of 80 W / cm and an energy of 100 mJ / cm. 2 This was then left at room temperature for one day, after which the base film on the second liquid crystal retardation layer film side was removed.

[0120] Through this, a polarizing plate was manufactured in which the third protective layer / adhesive layer (formed with an aqueous adhesive composition for polarizing plates, thickness: 100 nm) / polarizer / adhesive layer (formed with an aqueous adhesive composition for polarizing plates, thickness: 100 nm) / liquid crystal retardation layer (having a λ / 2 retardation at a wavelength of 550 nm) / adhesive layer (formed with a photocurable adhesive composition for polarizing plates, thickness: 3 μm) / liquid crystal retardation layer (having a λ / 4 retardation at a wavelength of 550 nm) were laminated in this order.

[0121] Examples 2 to 6 A polarizing plate was manufactured by carrying out the same method as in Example 1, except that the type and / or content of each component in the aqueous adhesive composition for polarizing plate in Example 1 was changed as shown in Table 1 below (unit: weight part).

[0122] Example 7 A polarizing plate was manufactured in the same manner as in Example 1, except that the aqueous adhesive composition for polarizing plate manufactured in Example 1 was used instead of the photocurable adhesive composition for polarizing plate in Example 1. Through this, a polarizing plate was manufactured in which the third protective layer / adhesive layer (formed with the aqueous adhesive composition for polarizing plate, thickness: 100 nm) / polarizer / adhesive layer (formed with the aqueous adhesive composition for polarizing plate, thickness: 100 nm) / liquid crystal retardation layer (having a λ / 2 retardation at a wavelength of 550 nm) / adhesive layer (formed with the aqueous adhesive composition for polarizing plate, thickness: 100 nm) / liquid crystal retardation layer (having a λ / 4 retardation at a wavelength of 550 nm) were laminated in this order.

[0123] Comparative Example 1 and Comparative Example 2 The adhesive composition for polarizing plates, laminates, and polarizing plates were prepared by carrying out the same method as in Example 1, except that the type and / or content of each component in the aqueous adhesive composition for polarizing plates in Example 1 was changed as shown in Table 1 below (unit: weight part).

[0124] Comparative Example 3 and Comparative Example 4 The same method as in Example 1 was carried out, except that the type and / or content of each component in the aqueous adhesive composition for polarizing plates in Example 1 was changed as shown in Table 1 below (unit: part by weight).

[0125] The compositions of the polarizing plate adhesives used in the examples and comparative examples are as shown in Table 1 below.

[0126] [Table 1]

[0127] In Table 1, A: Polyvinyl alcohol resin (Mitsubishi Chemical Corporation, Z200, polyvinyl alcohol modified with acetoacetyl groups, average polymerization degree: 1200, saponification degree: 99 mol%, acetoacetyl group modification degree: 5 mol%) B: Poly(ethyleneimine)-based crosslinking agent (Nippon Shokubai Co., Ltd., SP018, having a primary amine group or a secondary amine group) C: Glyoxal-based crosslinking agent (TCL Corporation, solid content 40% by weight, solvent is water) D: Zirconium compound (Zircosol-ZN, solvent is water, Daiichi Kigenso Kagaku Kogyo Co., Ltd.) E: Poly(ethylene glycol) diglycidyl ether (EX821, Nagase ChemteX Corporation) F: Ethylene glycol diglycidyl ether (EX811, Nagase ChemteX Corporation) G: Poly(propylene glycol) diglycidyl ether (EX920, Nagase ChemteX Corporation) The adhesives for polarizing plates and the polarizing plates of the Examples and Comparative Examples were evaluated for the following physical properties, and the results are shown in Table 2 below.

[0128] (1) Presence or absence of transfer of liquid crystal retardation layer: A laminate of COP film / adhesive layer / polarizer / adhesive layer (formed with a water-based adhesive for polarizing plate) / first liquid crystal retardation film (liquid crystal retardation layer / TAC film) was produced in the same manner as in the examples and comparative examples. After one hour had passed, when the TAC film was peeled off from the liquid crystal retardation layer, the case where the TAC film was peeled off from the liquid crystal retardation layer and the liquid crystal retardation layer was attached to the polarizer side was evaluated as "○", and the case where the liquid crystal retardation layer was separated from the polarizer was evaluated as "X".

[0129] (2) High temperature and high humidity durability: The polarizing plates prepared in the examples and comparative examples were cut into a length x width (50 mm x 50 mm) such that the absorption axis direction of the polarizer was in a 45° direction (diagonal direction), and then attached to a glass plate to prepare a test specimen. The prepared test specimen was left in a chamber at 60°C and 95% relative humidity for 500 hours. Referring to Figure 3, the average value of the length of four bleached regions 5 of the polarizer measured in a 45° direction (corner of the polarizer) to the length or width of the test specimen 1 was measured. The obtained average value was evaluated according to the following criteria.

[0130] ○: Less than 1mm △: 1mm or more, less than 3mm X: Exceeding 3mm.

[0131] (3) Bending Reliability: The polarizing plates manufactured in the examples and comparative examples were used to manufacture square test pieces with length x width (50 mm x 50 mm) so that the absorption axis direction of the polarizer was in the 45° direction (diagonal direction). As shown in FIG. 4, the manufactured test pieces 10 were folded in half so that the radius of curvature was 3R, and then placed between two slits 20 with a fixed shape. The test pieces were then placed in a chamber at 60°C and 95% relative humidity, and left for 500 hours before being removed. When no bubbles, wrinkles, wavy patterns, etc. were generated at the folded part due to lifting at the interlayer interface, the test pieces were evaluated as "○", and when even a small amount of bubbles, wrinkles, wavy patterns, etc. were generated, the test pieces were evaluated as "X".

[0132] [Table 2]

[0133] As shown in Table 2, the adhesive composition for polarizing plate of the present invention has excellent adhesive strength between the polarizer and the liquid crystal retardation layer, so that the transfer of the liquid crystal retardation layer is performed well. Thus, the present invention formed an adhesive layer having excellent high temperature and high humidity durability and bending reliability.

[0134] On the other hand, the adhesive compositions for polarizing plates of the comparative examples, which do not satisfy the constitution of the present invention, could not obtain all the effects of the present invention. In the comparative examples 3 and 4, the first liquid crystal retardation layer was separated from the polarizer during the process of removing the TAC film from the film for the first liquid crystal retardation layer, and a polarizing plate could not be manufactured.

[0135] Simple modifications and variations of the present invention can be easily implemented by those having ordinary skill in the art, and all such modifications and variations can be considered to be included within the scope of the present invention.

Claims

1. Polyvinyl alcohol resin, primary amine group (-NH 2 ) or a crosslinker having a secondary amine group (-NH-), and an epoxy compound having an alkylene oxide group, The polyvinyl alcohol-based resin includes a polyvinyl alcohol-based resin containing an acetoacetyl group, The epoxy compound having an alkylene oxide group includes at least one of poly(ethylene glycol) diglycidyl ether; propylene glycol diglycidyl ether; and poly(propylene glycol) diglycidyl ether. An adhesive composition for polarizing plates.

2. The adhesive composition for polarizing plates according to claim 1 , wherein the crosslinking agent having a primary amine group or a secondary amine group comprises at least one ethyleneimine-based crosslinking agent.

3. 2. The adhesive composition for polarizing plates according to claim 1, wherein the crosslinking agent and the epoxy compound having an alkylene oxide group are contained in a weight ratio of 1:1 to 1:

15.

4. 2. The adhesive composition for polarizing plates according to claim 1, wherein the alkylene oxide group is *-[-O-R-]-* (* is a linking moiety, and R is a linear or branched alkylene group having 2 to 4 carbon atoms).

5. The adhesive composition for polarizing plates according to claim 1 , wherein the epoxy compound having an alkylene oxide group further comprises ethylene glycol diglycidyl ether.

6. The composition comprises:

2. The adhesive composition for polarizing plates according to claim 1, comprising: 100 parts by weight of the polyvinyl alcohol-based resin; 0.1 to 50 parts by weight of the crosslinking agent having a primary amine group or a secondary amine group; and 1 to 100 parts by weight of the epoxy-based compound having an alkylene oxide group.

7. a polarizer; a first liquid crystal retardation layer laminated on a lower surface of the polarizer; and a first adhesive layer that adheres the polarizer and the first liquid crystal retardation layer; A polarizing plate, wherein the first adhesive layer is formed from the adhesive composition for polarizing plates according to claim 1 .

8. The polarizing plate according to claim 7 , wherein the first liquid crystal retardation layer contains an aromatic ring-containing liquid crystal compound.

9. The polarizing plate of claim 7 , further comprising a second adhesive layer and a second liquid crystal retardation layer laminated on a lower surface of the first liquid crystal retardation layer.

10. The polarizing plate according to claim 9 , wherein the second liquid crystal retardation layer contains an aromatic ring-containing liquid crystal compound.

11. 10. The polarizing plate of claim 9, wherein the second adhesive layer is formed of an adhesive composition for a polarizing plate, the adhesive composition comprising a polyvinyl alcohol-based resin, a crosslinking agent having a primary amine group or a secondary amine group, and an epoxy-based compound having an alkylene oxide group.

12. The polarizing plate according to claim 11, wherein the crosslinking agent having a primary amine group or a secondary amine group includes at least one ethyleneimine-based crosslinking agent.

13. The polarizing plate according to claim 11, wherein the epoxy compound having an alkylene oxide group comprises at least one of ethylene glycol diglycidyl ether; poly(ethylene glycol) diglycidyl ether; propylene glycol diglycidyl ether; and poly(propylene glycol) diglycidyl ether.

14. An optical display device comprising the polarizing plate of claim 7.

Citation Information

Patent Citations

  • Adhesive and glass base

    JP1991045678A

  • Microcapsule type adhesive particle for adhesion of liquid crystal display panel board

    JP1998219222A

  • Compound polarizing plate

    JP2006235613A

  • Polarizing plate

    JP2007256501A

  • Adhesive retardation layer-stuck polarizing plate, optical film and image display device

    JP2011013684A