Method for Making Plaster-Based Products
Incorporating fine particle distributed polyvinyl acetate into the gypsum matrix enhances the anchoring strength of gypsum-based panels, addressing the secure attachment of fixtures without additional materials, achieving high screw pullout strength and efficient installation.
Patent Information
- Application Number
- JP2021520192
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-11-15
- Filing Date
- 2019-11-07
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2039-11-07
AI Technical Summary
Lightweight gypsum-based panels struggle to securely attach fixtures due to insufficient anchoring strength, requiring additional materials like plywood or metal supports that increase weight, thickness, and installation complexity.
Incorporating fine particle distributed polyvinyl acetate into the gypsum matrix of gypsum-based products, with a particle size distribution where 90% of particles are 4.5 μm or less, enhances anchoring strength without additional components.
The method significantly increases the screw pullout strength of gypsum-based products to at least 550N, reducing the need for additional supports and simplifying installation.
Smart Images

Figure 0007595568000002 
Figure 0007595568000003 
Figure 0007595568000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for making a gypsum-based product containing a polymeric additive, and more particularly to a method for making a gypsum-based product containing polyvinyl acetate.
[0002] Lightweight panels such as plasterboard (e.g. gypsum board), polystyrene board and fibreboard are commonly used to provide partitions within buildings and their advantages in the context of this application include being light and quick to install.
[0003] However, in certain cases such lightweight panels may have the drawback that they are not strong enough to support fixtures (e.g. sinks, televisions, radiators, fire extinguishers, shelves and any other items requiring attachment to the panel) when the fixing means (e.g. screws) are inserted directly into the panel, i.e. in the absence of inserts such as wall plugs or anchors. In such cases the weight of the fixture may pull the fixing means (e.g. screws) out of the panel, causing the fixture to fall off the partition.
[0004] Typically, this problem has been addressed by providing a plywood sheet to increase the fixing strength of the panel, where the plywood sheet is provided on the side of the panel opposite the side on which the fixture is to be installed. The plywood sheet provides additional strength to hold one or more fixing means (e.g. screws) used to secure the fixture to the panel. Typically, the plywood sheet is placed within the framework of the partition and then the plasterboard is secured to the plywood so that it is located on the outside of the framework of the partition.
[0005] Alternatively, metal support means may be provided. These may include fixing plates, channels, straps or metal fasteners. As in the case of plywood sheets, the metal support means will generally be located on the side of the panel opposite to the side to which the fixture is secured and will serve to receive and secure the fastening means, e.g. fastening screws used to attach the fixture to the panel.
[0006] Both of these configurations have the disadvantage that the panel and further support components must be attached to each other on-site. Furthermore, if metal support means are used, multiple such support means may be required to support the set of fastening means required to secure the fixture to the panel. The installation process may therefore be time consuming and expensive.
[0007] Furthermore, the addition of metal support means or plywood sheets increases the weight and thickness of the partition and / or causes a reduction in the cavity wall space. The plywood itself generally must be cut to size on-site, thus increasing the time required for installation and possibly resulting in the release of dust and potentially harmful components.
[0008] Therefore, there is a need to provide an improved panel that can retain fastening means to support fixtures and that does not require a time consuming installation process.
[0009] It has previously been found that incorporating polymers and / or fibers into the gypsum matrix of a gypsum board can help to increase the anchorage strength of the board. Typically, a polymer and / or fiber component is mixed into the gypsum slurry used to form the plasterboard.
[0010] Surprisingly, it has been found that when polyvinyl acetate is incorporated into the gypsum matrix of a gypsum-based product, the anchoring strength of the gypsum-based product can be increased even further if the polyvinyl acetate is provided in the form of a particulate distribution.
[0011] Accordingly, in a first aspect, the invention can provide a method of making a gypsum-based product comprising mixing gypsum with polymer particles and water to obtain a slurry, the polymer particles comprising primarily polyvinyl acetate, the polymer particles having a particle size distribution, as measured using laser diffraction, such that at least 90% of the total particle volume of the polymer particles are particles having a diameter of 4.5 μm or less.
[0012] Typically, the polymer particles are incorporated into the slurry in the form of an aqueous emulsion. In such cases, the method may further comprise the step of incorporating an additional amount of water into the slurry in addition to the aqueous emulsion.
[0013] In a less preferred alternative, the polymer particles may be incorporated into the slurry in dry form and water may be provided separately to form the slurry.
[0014] The particle size distribution of the polymer particles is determined using laser diffraction measurement of the particle size when the particles are suspended in an aqueous emulsion.
[0015] Preferably, the polymer particles have a particle size distribution, as measured using laser diffraction, such that particles having a diameter of 4 μm or less account for at least 90% of the total particle volume.
[0016] More preferably, the polymer particles have a particle size distribution, as measured using laser diffraction, such that particles having a diameter of 3.5 μm or less account for at least 90% of the total particle volume.
[0017] In certain cases, the particle size distribution of the polymer particles is unimodal (also known as monomodal).
[0018] Typically, the particles have an average polyvinyl acetate content of at least 80% by volume, preferably 85% by volume, and more preferably 90% by volume.
[0019] In certain cases, the particles further comprise polyvinyl alcohol, which may be present as a surface layer extending partially or entirely around the outer surface of the particle. The presence of polyvinyl alcohol is typically believed to be due to partial hydrolysis of polyvinyl acetate. It is believed that the presence of polyvinyl alcohol may help stabilize the polymer particles.
[0020] Typically, the polymer particles are present in the slurry in an amount of at least 1 wt. % relative to the gypsum, preferably at least 3 wt. %, and most preferably at least 4 wt. %.
[0021] Typically, the polymer particles are present in the slurry in an amount of no more than 25 wt.% relative to the gypsum, preferably no more than 20 wt.%, and most preferably no more than 15 wt.%.
[0022] Plaster of Paris typically comprises calcium sulfate hemihydrate and / or calcium sulfate anhydrite. Calcium sulfate hemihydrate may exist in the alpha and / or beta forms.
[0023] Typically, the water content of the slurry (including any water provided as part of the emulsion of polymer particles and any water provided separately) is at least 40 wt.% relative to the calcined gypsum, preferably at least 50 wt.%, and most preferably at least 60 wt.% relative to the calcined gypsum. Generally, lower water contents (e.g., less than 40 wt.%) are achievable when all or most of the calcium sulfate hemihydrate is present in the alpha form, e.g., when at least 50 wt.% of the calcium sulfate hemihydrate is present in the alpha form. Typically, higher water contents (e.g., at least 60 wt.%) are required when all or most of the calcium sulfate hemihydrate is present in the beta form, e.g., when at least 50 wt.% of the calcium sulfate hemihydrate is present in the beta form.
[0024] Typically, the water content of the slurry is less than 120 wt. % relative to the gypsum, and preferably less than 100 wt.
[0025] Typically, the method further comprises incorporating a fibrous reinforcement, such as glass fibres, into the slurry. In certain cases, the fibres of the fibrous reinforcement have an average length in the range of 2 to 20 mm, typically 5 to 15 mm. Generally, the fibrous reinforcement is present in the slurry in an amount of at least 1 wt. %, preferably at least 1.5 wt. %, more preferably at least 2 wt. %, relative to the gypsum.
[0026] Typically, the fibrous reinforcement is present in the slurry in an amount of no more than 15 wt.% relative to the calcined gypsum, preferably no more than 10 wt.%, and most preferably no more than 5 wt.%.
[0027] Typically, the method is used to make a board having a core of a gypsum matrix. Typically, the board is provided with a liner, such as a paper liner or a fiberglass mat, on at least one side. The liner is typically partially or fully embedded in the board. That is, the gypsum slurry typically partially or fully penetrates the liner during setting of the gypsum slurry to form the board.
[0028] Typically the board has a screw pull-out strength of at least 550N, preferably at least 600N.
[0029] Other non-hazardous materials, adjuvants and ingredients may be included in the slurry as desired. Such non-hazardous materials may include optional additional ingredients such as polymers other than polyvinyl acetate or polyvinyl alcohol (including other synthetic polymers and / or starches), set accelerators and retarders, deformation inhibitors (such as anti-sag agents), anti-shrinkage additives, recalcination inhibitors, foam stabilizers, bactericides, fungicides, pH adjusters, colorants, flame retardants, hydrophobic additives and fillers (such as particulate inorganic materials or plastics that may be foamed in some embodiments).
[0030] The invention will now be described by way of example with reference to the following figures: [Brief description of the drawings]
[0031] [Figure 1a] 1 shows a graphical representation of particle size distribution of Example 1. [Figure 1b] 1 shows a graphical representation of particle size distribution of Example 2. [Figure 1c] 1 shows a graphical representation of particle size distribution of Example 3. [Figure 1d] 1 shows a graphical representation of particle size distribution of Example 4. [Figure 1e] 1 shows a graphical representation of particle size distribution of Example 5. [Figure 1f] 1 shows a graphical representation of particle size distribution of Example 6. [Figure 1g] 1 shows a graphical representation of particle size distribution of Example 7. [Figure 1h] 1 shows a graphical representation of particle size distribution of Example 8. [Figure 1i] 1 shows a graphical representation of particle size distribution for Comparative Example 9. [Figure 1j] 1 shows a graphical representation of particle size distribution for Comparative Example 10. [Figure 1k] 1 shows a graphical representation of particle size distribution for Comparative Example 11. [Diagram 2] The screw pull-out data for Examples 1 to 8 and Comparative Examples 9 to 11 are shown. EXAMPLES
[0032] The volume-based particle size distributions of eleven samples of aqueous polyvinyl acetate emulsions were determined and used to calculate the D 90 values were calculated.
[0033] These emulsions were then incorporated into respective gypsum-based slurries in an amount sufficient to provide a polyvinyl acetate content of 4.5 wt.% relative to the gypsum (measured by dry weight of polyvinyl acetate). The slurries also contained fiber in an amount of 2.3 wt.% relative to the gypsum and had a total water content sufficient to provide a water content of 80 wt.% relative to the gypsum. Each slurry was then formed into a respective gypsum board. The screw pull strength of each board was determined.
[0034] The results are shown in Table 1. In addition, graphical representations of the volume-based particle size distributions of each polyvinyl acetate sample are shown in Figure 1(a)-(k), and the screw pull-out results are displayed graphically in Figure 2. [Table 1]
[0035] D 90 Measurement of values Volume-based particle size distributions of aqueous polyvinyl acetate dispersions were measured using laser diffraction using a Malvern Mastersizer 3000 laser diffraction particle sizer.
[0036] Polyvinyl acetate samples were diluted in water to produce an emulsion containing 4.5 wt% polyvinyl acetate based on solids. The emulsion was shaken manually for 1 minute to ensure uniform dispersion of the polymer and then pipetted into the dispersion unit of the measurement instrument. The polymer emulsion was added in an amount to produce an obscuration of 1% to 4%. The dispersion unit was stirred at 3000 ± 50 rpm.
[0037] The measurement device was operated in spherical particle mode.
[0038] Three samples were tested for each Example and Comparative Example, and six particle size distribution traces were performed for each sample. Thus, 18 tests were performed for each Example and Comparative Example. 90 Values represent the average taken from these 18 tests. The graphical representations of particle size distributions shown in Figures 1(a)-1(k) represent the average of six traces taken from one of the samples.
[0039] Preparation of gypsum board samples In preparing the gypsum board samples, a gypsum slurry was prepared from stucco (plaster of Paris), glass fibers having an average length of 6 mm, an aqueous polyvinyl acetate emulsion, and additional water.
[0040] The fiber content of the slurry was 2.3 wt% relative to the stucco. The polyvinyl acetate emulsion was added to the slurry in an amount to obtain a polyvinyl acetate content of 4.5 wt% relative to the stucco, excluding the water present in the emulsion. The water content of the slurry (including the water from the polyvinyl acetate emulsion and additional water) was 80 wt% relative to the stucco.
[0041] A slurry was prepared by hand mixing the required amount of aqueous polyvinyl acetate emulsion with additional water. The fibers were then added to the diluted emulsion and mixed for 30 seconds using a Kenwood mixer. Stucco was then added to the aqueous polyvinyl acetate / fiber mixture in the Kenwood mixer and mixed for 30 seconds.
[0042] The slurry was poured into a mold having opposing sides defining a flat cavity. The opposing sides of the cavity were lined with water-saturated paper. The mold was supported with the cavity facing upwards. The exterior surface of the mold was tapped lightly to remove any air pockets in the slurry, and additional slurry was poured into the cavity as needed until it was full.
[0043] The slurry was left to set for 15-20 minutes, after which the mold was opened and the gypsum board removed. Any excess paper was cut from the edges of the board and masking tape was wrapped around the edges of the board.
[0044] 25 minutes after the slurry was poured into the mold, the board was placed in an oven at 160° C. for 1 hour. The board was then removed from the oven, the masking tape was removed from the edges of the board, and the board was placed in another oven at 40° C. for approximately 24 hours until a constant weight was reached.
[0045] After this, the boards were conditioned at 23° C. and 50% relative humidity for approximately 24 hours until a constant weight was reached.
[0046] Screw pull-out strength measurement In the screw pull-out test, a universal testing machine is used to apply a pull-out force to a screw embedded in a board until the screw is removed from the board.
[0047] Screw pull-out tests were performed on the conditioned boards using Unifix single start screws with a 50mm long and 5mm diameter shaft. Before the pull-out test began, the screws were inserted into the board so that 10mm (±1mm) of the screw extended from the rear of the board. After a preload of 10N was applied, the load was increased at a crosshead speed of 10mm / sec until failure. The peak failure load was recorded to obtain the pull-out strength.
Claims
1. 1. A method of making a gypsum-based product, comprising mixing gypsum with polymer particles and water to obtain a slurry, the polymer particles comprising polyvinyl acetate such that the particles have an average polyvinyl acetate content of at least 80% by volume; the polymer particles have a particle size distribution, as measured using laser diffraction, such that particles having a diameter of 4.5 μm or less account for at least 90% of the total particle volume; the particles further comprise polyvinyl alcohol, and the polyvinyl alcohol phase is present as a surface layer extending partially or entirely around an outer surface of the particles; The polymer particles are present in the slurry in an amount of 15 wt % or less relative to the gypsum. method.
2. 10. The method of claim 1, wherein the polymer particles have a particle size distribution, as measured using laser diffraction, such that particles having a diameter of 4 μm or less account for at least 90% of the total particle volume.
3. 3. The method of claim 2, wherein the polymer particles have a particle size distribution, as measured using laser diffraction, such that particles having a diameter of 3.5 μm or less account for at least 90% of the total particle volume.
4. The method of any one of claims 1 to 3, wherein the particles have an average polyvinyl acetate content of at least 90% by volume.
5. The method according to any one of claims 1 to 4, wherein the polymer particles are provided in the form of an aqueous emulsion.
6. The method of any one of claims 1 to 5, wherein the polymer particles are present in the slurry in an amount of at least 1 wt % relative to the gypsum.
7. The method of any one of claims 1 to 6, further comprising the step of incorporating fibers into the slurry.
8. 8. The method of claim 7, wherein the fibers are present in the slurry in an amount of at least 1 wt.% relative to the gypsum.
9. The method according to any one of claims 1 to 8, wherein the gypsum-based product is a board.
10. The method of claim 9 , wherein the board has a liner on at least one surface.
11. The method according to any one of claims 1 to 10, further comprising forming the slurry and hardening it to obtain a gypsum board.
Citation Information
Patent Citations
Structural panels with improved fixing strength
JP2017536318A
Structural panel with improved fixing strength