Borophosphate compounds and borophosphate nonlinear optical crystals, and their preparation methods and uses

Alkali metal borophosphate crystals address the challenges of deep UV nonlinear optical crystals by providing high transparency and birefringence, enabling efficient frequency multiplication and easy growth, suitable for nonlinear optical devices.

JP7595965B2Active Publication Date: 2024-12-09TIANJIN UNIVERSITY OF TECHNOLOGY
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023044488
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-08-26
Filing Date
2023-03-20
Publication Date
2024-12-09
Estimated Expiration
2043-03-20

AI Technical Summary

Technical Problem

The challenge lies in developing deep ultraviolet nonlinear optical crystals that meet stringent requirements of non-centrosymmetric structure, high transparency, large second-order nonlinear optical coefficient, moderate birefringence, and easy growth, while overcoming the limitations of conventional materials with small frequency multiplication response and birefringence.

Method used

The development of alkali metal borophosphate compounds, specifically A3B11P2O23 (where A=K, Rb, Cs, NH4), synthesized through solid phase, hydrothermal, or solution methods, which possess a trigonal structure and no center of symmetry, enabling high transparency and birefringence suitable for deep UV applications.

Benefits of technology

The alkali metal borophosphate crystals exhibit wide light transmission frequency bands, high hardness, and excellent mechanical properties, facilitating easy crystal growth and processing, making them suitable for nonlinear optical devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007595965000003
    Figure 0007595965000003
  • Figure 0007595965000004
    Figure 0007595965000004
  • Figure 0007595965000005
    Figure 0007595965000005
Patent Text Reader

Abstract

To provide a series of alkali metal borophosphates compounds, and alkali metal borophosphates nonlinear optical crystals as well as a preparation method and application thereof.SOLUTION: In the present invention, chemical formulas of a series of compounds and crystals thereof are all A3B11 P2O23, wherein A=K, Rb, Cs, NH4 is K3B11 P2O23, Rb3B11 P2O23, Cs3B11 P2O23, or (NH4)3B11 P2O23. The series of crystals belong to trigonal system, space group R3, and unit cell parameters are Z=3. The series of alkali metal borophosphate compounds are synthesized by using a solid phase reaction method or a hydrothermal method, and the series of nonlinear optical crystals are grown by using a high-temperature melt method, a hydrothermal method or a solution method. The series of materials can be used for manufacturing second harmonic generators, up and down frequency converters, optical parametric oscillators, and the like.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a series of alkali metal borophosphate compounds and methods for preparing alkali metal borophosphate nonlinear optical crystals and nonlinear optical devices fabricated utilizing said series of crystals. [Background technology]

[0002] Deep-UV coherent light with wavelengths of 200-150 nm is becoming increasingly important due to its potential applications in semiconductor photolithography, laser micromachining and modern scientific instruments. For solid-state lasers, obtaining deep-UV coherent light is achieved by cascade frequency conversion techniques in nonlinear optical crystals. However, for the deep-UV nonlinear optical crystals to be applied, they must have i) a non-centrosymmetric structure, ii) at least the d of KDP. 36 and the corresponding large second-order nonlinear optical coefficient (d ij ), iii) high transparency in the deep ultraviolet region with the shortest possible ultraviolet cutoff wavelength, iv) moderate birefringence (△n=0.05-0.10) to meet the phase-matching condition of second harmonic generation in the ultraviolet or deep ultraviolet region, and v) it must meet stringent structure and performance requirements, including easy growth, non-toxicity, chemical stability and good mechanical properties. However, due to the contradiction of some of the above attributes, large band gap materials often exhibit small frequency doubling response and birefringence, and the design and synthesis of deep ultraviolet nonlinear optical crystals remains a huge challenge.

[0003] Borophosphates with asymmetric [BO4] and [PO4] tetrahedra as basic structural units usually have large band gaps and are widely considered as candidate materials for exploring UV or DUV optical crystals. Notably, BPO4 has a strong second harmonic response (2×KDP) and its UV transmittance range extends to about 130 nm. However, the birefringence is very small at 0.005@1064 nm, which makes conventional phase matching impossible and the crystal cannot be used as an ultraviolet nonlinear optical crystal. However, the π-conjugated [BO3] group with excellent optical anisotropy is beneficial for improving the birefringence of the material. Therefore, designing and synthesizing borophosphates with [BO3], [BO4] and [PO4] groups is an effective means to design deep ultraviolet nonlinear optical materials. Summary of the Invention [Problem to be solved by the invention]

[0004] A primary object of the present invention is to provide a series of alkali metal borophosphate compounds and methods of preparation.

[0005] A second object of the present invention is to provide a series of alkali metal borophosphate nonlinear optical crystals and preparation methods.

[0006] A third object of the present invention is to provide applications for a series of alkali metal borophosphate nonlinear optical crystals. [Means for solving the problem]

[0007] The first object of the present invention is achieved as follows.

[0008] The present invention provides a series of alkali metal borophosphate compounds, the chemical formula of which is A3B 11 P2O 23 (A = K, Rb, Cs, NH4), and the molecular formula is K3B 11 P2O 23 , Rb3B 11 P2O 23 , Cs3B11 P2O 23 or (NH4)3B 11 P2O 23 and the molecular weights are 666.15, 805.26, 947.57 and 602.97, respectively. A series of alkali metal borophosphate compounds are prepared according to the following chemical reaction formulas by using a solid-state reaction method, a hydrothermal method or a solution method.

[0009] 1)3A2CO3(A=K, Rb, Cs, NH4)+22H3BO3+4NH4H2PO4→2A3B 11 P2O 23 (A=K, Rb, Cs, NH4)+39H2O↑+3CO2↑+4NH3↑ 2)3AOH(A=K, Rb, Cs, NH4)+11H3BO3+P2O5→A3B 11 P2O 23 (A=K, Rb, Cs, NH4)+18H2O↑ 3)3A2CO3(A=K, Rb, Cs, NH4)+22H3BO3+2P2O5→2A3B 11 P2O 23 (A=K, Rb, Cs, NH4)+33H2O↑+3CO2↑ 4)3A2O(A=K, Rb, Cs, NH4)+22H3BO3+2P2O5→2A3B 11 P2O 23 (A=K, Rb, Cs, NH4)+33H2O↑ 5)3AF(A=K,Rb,Cs,NH4)+11H3BO3+2NH4H2PO4→A3B 11 P2O 23 (A=K, Rb, Cs, NH4)+18H2O↑+3HF↑+2NH3↑ 6)3A2CO3(A=K, Rb, Cs, NH4)+11B2O3+4NH4H2PO4→2A3B 11 P2O 23 (A=K, Rb, Cs, NH4)+6H2O↑+3CO2↑+4NH3↑ 7)3A2CO3(A=K, Rb, Cs, NH4)+11B2O3+2P2O5→2A3B 11 P2O 23 (A=K, Rb, Cs, NH4)+3CO2↑ 8)3AH2PO4(A=K,Rb,Cs,NH4)+5.5B2O3→A3B 11 P2O 23 (A=K, Rb, Cs, NH4)+1.5H2O↑+H3PO4 9)3A2HPO4(A=K, Rb, Cs, NH4)+11B2O3+0.5P2O5→2A3B 11 P2O 23 (A=K, Rb, Cs, NH4)+1.5H2O↑ 10)6AOH(A=K, Rb, Cs, NH4)+11B2O3+2P2O5→2A3B 11 P2O 23 (A=K, Rb, Cs, NH4)+3H2O↑ 11)12AH2PO4(A=K, Rb, Cs, NH4)+22H3B2O3+2P2O5→4A3B 11 P2O 23 (A=K, Rb, Cs, NH4)+33H2↑+8H3PO4 12)6ACl(A=K, Rb, Cs, NH4)+11B2O3+4NH4H2PO4→2A3B 11 P2O 23 (A=K, Rb, Cs, NH4)+6HCl↑+4NH3↑+3H2O↑ 13)6ACl(A=K,Rb,Cs,NH4)+22H3BO3+2P2O5→2A3B 11 P2O 23 (A=K, Rb, Cs, NH4)+6HCl↑+30H2O↑

[0010] The second object of the present invention is achieved as follows.

[0011] The present invention aims to provide a series of alkali metal borophosphate nonlinear optical crystals, the chemical formula of which is A3B 11 P2O 23 where A = K, Rb, Cs, NH4, has no center of symmetry, is trigonal, and belongs to the space group R3. The unit cell parameters are [ka] , α = 90°, β = 90°, γ = 120°, Z = 3. A series of alkali metal borophosphate nonlinear optical crystals are grown using high temperature melt, hydrothermal or solution techniques.

[0012] Using the high-temperature melting method, A3B 11 P2O 23 where A = K, Rb, Cs, and NH4 are nonlinear optical crystals with the molecular formulas K3B 11 P2O 23 , Rb3B 11 P2O 23 , Cs3B 11 P2O 23 or (NH4)3B 11 P2O 23 The specific operations are carried out according to the following steps:

[0013] a. Mix the single-phase polycrystalline powder of a series of alkali metal borophosphate compounds and flux uniformly, heat to a temperature of 350-800°C, keep at a constant temperature for a certain period of time to obtain a mixed molten liquid, and then cool to a temperature of 300-750°C, where the molar ratio of the single-phase polycrystalline powder of a series of alkali metal borophosphate compounds and flux is 1:0-20.

[0014] Alternatively, a mixture of A=K, Rb, Cs, NH4-containing compound, boron-containing compound and phosphorus-containing compound, or a mixture of A=K, Rb, Cs, NH4-containing compound, boron-containing compound and phosphorus-containing compound and flux is directly heated to a temperature of 350-800°C, kept at a constant temperature for a certain period of time to obtain a mixed molten liquid, and then cooled to a temperature of 300-750°C, where the molar ratio of A=K, Rb, Cs, NH4-containing compound, boron-containing compound, phosphorus-containing compound and flux is 2.5-3.5:10.5-11.5:1.5-2.5:0-20.

[0015] The flux mainly comprises at least one or more of alkali metal salts, i.e., alkali metal carbonates, alkali metal nitrates, alkali metal sulfates, alkali metal oxalates, alkali metal borates, alkali metal phosphates, alkali metal halides, alkali metal fluoroborates, alkali metal metaborates, and alkali metal oxides, alkali metal hydroxides, and monohydrogen phosphates, dihydrogen phosphates, boron oxide, boric acid, phosphoric acid, lead oxide, lead fluoride, molybdenum oxide, and bismuth oxide.

[0016] The single-phase polycrystalline powders of the series of alkali metal borophosphate compounds are prepared using a solid-state synthesis method, which includes the following steps: Mix A=K, Rb, Cs, NH4-containing compound, boron-containing compound and phosphorus-containing compound, and use solid-state reaction method to prepare a series of alkali metal borophosphates of the above compounds, the molar ratio of A=K, Rb, Cs, NH4-containing compound, ...

[0017] b. Preparation of a series of alkali metal borophosphate seed crystals: The mixed melt obtained in step a is gradually cooled to room temperature, and spontaneously crystallized to obtain a series of alkali metal borophosphate seed crystals.

[0018] c) Place the crucible containing the mixed melt prepared in step a in a crystal growth furnace, fix the seed crystal obtained in step b to a seed crystal rod, lower the seed crystal from the top of the crystal growth furnace, preheat the seed crystal rod, and then melt back the seed crystal until it touches the liquid surface of the mixed melt or lower it into the mixed melt, maintain the temperature for a certain period of time, and then gradually lower the temperature to the saturation temperature.

[0019] d. The temperature is then gradually decreased, and the seed crystal rod is rotated to grow the crystal. After the single crystal grows to a required size, the crystal is lifted from the surface of the mixed melt and gradually decreased to room temperature. Then, the crystal is removed from the hearth to obtain a series of alkali metal borophosphate nonlinear optical crystals.

[0020] Using the hydrothermal method, A3B 11 P2O 23 The growth of the nonlinear optical crystal is carried out according to the following steps:

[0021] a, A=K, Rb, Cs, NH4-containing compound, boron-containing compound and phosphorus-containing compound are added to the polytetrafluoroethylene lining of the autoclave, and 0.1-50 mL of deionized water or 0.1-50 g of mineralizer are further added and mixed thoroughly and uniformly to obtain a mixed solution, where the molar ratio of A=K, Rb, Cs, NH4-containing compound, boron-containing compound and phosphorus-containing compound is 2-4:10-12:1-3.

[0022] b. The polytetrafluoroethylene-lined lid containing the mixed solution from step a is tightened, and the lid is placed in a corresponding autoclave, and the piston of the autoclave is tightened.

[0023] c) The autoclave from step b is placed in a thermostatic chamber, heated to 120 to 330° C., kept at that temperature for a certain period of time, and then cooled to room temperature.

[0024] d, the autoclave is opened and the solution containing the crystals is filtered to obtain a series of transparent alkali metal borophosphate nonlinear optical crystals.

[0025] Using the solution method, A3B 11 P2O 23 The growth of the nonlinear optical crystal is carried out according to the following steps:

[0026] Add A=K, Rb, Cs, NH4-containing compound, boron-containing compound and phosphorus-containing compound to the beaker, add 0.1-400mL of deionized water and stir until the solution becomes transparent. Then, place the beaker on a heating table and heat the temperature to 25-400℃, and after a certain time, obtain the series of alkali metal borophosphate nonlinear optical crystals. To grow it further, suspend the seed crystals of the series of crystals in the solution with a thin platinum wire. To reduce water evaporation, cover the beaker with a polyethylene sheet and drill several tens of millimeter-sized holes on it. After a certain time, take out the series of alkali metal borophosphate nonlinear optical crystals of centimeter size from the solution.

[0027] The third object of the present invention is achieved as follows.

[0028] The series of alkali metal borophosphate nonlinear optical crystal products have the advantages of high purity, easy crystal growth, transparent and uncoated, fast growth rate, low cost, and easy to obtain large crystals. The obtained crystals have the advantages of a wide optical transmission frequency band, high hardness, excellent mechanical properties, not easily fractured or deliquesced, and easy to process and store. The series of alkali metal borophosphate nonlinear optical crystals obtained by the method according to the present invention can be used as a nonlinear optical device, including an apparatus for passing at least one incident electromagnetic radiation through at least one nonlinear optical device to generate at least one output radiation having a frequency different from that of the incident electromagnetic radiation, according to the application of the device, among which the nonlinear optical crystal is A3B 11 P2O 23 (A = K, Rb, Cs, NH4) crystals, and the molecular formula is K3B 11 P2O 23 , Rb3B 11 P2O 23 , Cs3B 11 P2O 23 or (NH4)3B 11 P2O 23 It is. [Brief description of the drawings]

[0029] [Figure 1] FIG. 2 is an XRD spectrum diagram of the compound Rb3B11P2O23 powder of the present invention. [Diagram 2] FIG. 2 is an XRD spectrum diagram of the compound Cs3B11P2O23 powder of the present invention. [Diagram 3] FIG. 1 is a crystal structure diagram of a series of alkali metal borophosphates A3B11P2O23, where A=K, Rb, Cs, NH4 of the present invention. [Figure 4] FIG. 1 is a diagram showing the working principle of the nonlinear optical device manufactured by the present invention, in which 1 is a laser, 2 is an emission beam, 3 is a series of alkali metal borophosphate nonlinear optical crystals, 4 is an output beam, and 5 is a filter. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0030] The present invention will be described in detail below with reference to the drawings and embodiments, but is not limited to the described embodiments. Any improvements and variations made based on the present invention are within the protection scope of the present invention.

[0031] Example 1

[0032] Reaction formula: 3A2CO3 (A = K, Rb, Cs, NH4) + 22H3BO3 + 4NH4H2PO4 → 2A3B 11 P2O 23 According to (A=K, Rb, Cs, NH4)+39H2O↑+3CO2↑+4NH3↑, A3B 11 P2O 23 (A=K, Rb, Cs, NH4) compounds were synthesized.

[0033] A2CO3 (A=K, Rb, Cs, NH4), H3BO3, P2O5 are weighed in a molar ratio of 3:22:4 and put into a mortar, mixed and ground well, then put into an open corundum crucible with a diameter of 100mm×100mm, put into a muffle furnace, gradually heated to 350℃, kept at a constant temperature for 24 hours, cooled to room temperature, taken out and ground for the second time, put into a muffle furnace, further heated to 550℃, kept at a constant temperature for 24 hours, cooled to room temperature, taken out and ground for the third time, put into a muffle furnace, kept at a constant temperature at 550℃ for 48 hours, ground and prepared single-phase polycrystalline powder of a series of alkali metal borophosphate compounds is taken out, and the product is subjected to X-ray analysis, and the obtained X-ray spectrum shows that the series of alkali metal borophosphate A3B 11 P2O 23 This was consistent with the X-ray spectrum obtained from the single crystal structure of (A = K, Rb, Cs, NH4).

[0034] The resulting series of alkali metal borophosphate compounds A3B 11 P2O 23 Single-phase polycrystalline powders of (A=K, Rb, Cs, NH4) were placed in an open platinum crucible with a diameter of 80 mm x 80 mm, heated to 650°C at a heating rate of 30°C / h, and kept at the same temperature for 3 hours to obtain a mixed molten liquid, which was then cooled to 610°C.

[0035] The temperature was gradually lowered to room temperature at a rate of 0.5°C / h, and spontaneous crystallization occurred to obtain a series of alkali metal borophosphate seed crystals.

[0036] Crystal growth in compound melts: A3B obtained 11 P2O 23 (A=K, Rb, Cs, NH4) A seed crystal was fixed to a seed crystal rod, lowered from the top of a crystal growth furnace, preheated on the surface of the mixed melt for 10 minutes, and then immersed in the liquid surface to melt back into the mixed melt, kept at a constant temperature for 30 minutes, and then rapidly cooled to the saturation temperature of 600°C.

[0037] The temperature was further decreased at a rate of 0.1°C / day, and the seed crystal rod was rotated at a rotation speed of 10 rpm. After the crystal growth was completed, the crystal was removed from the liquid surface and the temperature was decreased to room temperature at a rate of 10°C / h. 11 P2O 23 (A=K, Rb, Cs, NH4) crystals were obtained.

[0038] Example 2

[0039] Reaction formula: 3AOH (A = K, Rb, Cs, NH4) + 11H3BO3 + P2O5 → A3B 11 P2O 23 (A=K, Rb, Cs, NH4)+18H2O↑, A3B 11 P2O 23 (A=K, Rb, Cs, NH4) compounds were synthesized.

[0040] The raw materials AOH (A = K, Rb, Cs, NH4), H3BO3, and P2O5 were directly weighed out in a molar ratio of 3:11:1, and the weighed raw materials were mixed with the flux AOH (A = K, Rb, Cs, NH4)-P2O5 in a molar ratio of 1:4, where the molar ratio of AOH to P2O5 was 3:5. The mixture was placed in an open platinum crucible of Φ80mm x 80mm, heated to 800℃, and kept at a constant temperature for 60 hours to obtain a mixed molten liquid, which was then further cooled to 750℃.

[0041] The temperature was gradually lowered to room temperature at a rate of 1.5°C / h, and spontaneous crystallization occurred to obtain a series of alkali metal borophosphate seed crystals.

[0042] The obtained A3B 11 P2O 23 (A=K, Rb, Cs, NH4) A seed crystal was fixed to a seed crystal rod, lowered from the top of a crystal growth furnace, preheated on the surface of the mixed melt for 10 minutes, and then immersed below the liquid surface to melt back into the mixed melt, kept at a constant temperature for 30 minutes, and then rapidly cooled to the saturation temperature of 700°C.

[0043] The temperature was then gradually lowered at a rate of 1°C / day. The seed crystal rod was not rotated. After the crystal had grown to the required size, the crystal was lifted from the surface of the melt and cooled to room temperature at a rate of 20°C / h. The crystal was then removed from the hearth and placed in a 36mm x 22mm x 15mm A3B mold. 11 P2O 23 (A=K, Rb, Cs, NH4) crystals were obtained.

[0044] Example 3

[0045] Reaction formula: 3A2CO3 (A = K, Rb, Cs, NH4) + 22H3BO3 + 2P2O5 → 2A3B 11 P2O 23 According to (A=K, Rb, Cs, NH4) + 33H2O↑ + 3CO2↑, A3B 11 P2O 23 (A=K, Rb, Cs, NH4) compounds were synthesized.

[0046] The raw materials A2CO3 (A=K, Rb, Cs, NH4), H3BO3, and P2O5 were directly weighed out in a molar ratio of 3:22:2, and the weighed raw materials were mixed with the flux H3BO3-P2O5 in a molar ratio of 1:3, where the molar ratio of H3BO3 and P2O5 was 3:1. The materials were placed in an open platinum crucible of Φ80mm×80mm, heated to 350℃, and kept at a constant temperature for 60 hours to obtain a mixed molten liquid, which was then cooled to 330℃.

[0047] The temperature was gradually lowered to room temperature at a rate of 3.5°C / h, and spontaneous crystallization occurred to obtain a series of alkali metal borophosphate seed crystals.

[0048] The obtained A3B 11 P2O 23 (A=K, Rb, Cs, NH4) A seed crystal was fixed to a seed crystal rod, lowered from the top of a crystal growth furnace, preheated on the surface of the mixed melt for 15 minutes, and then immersed below the liquid surface to melt back into the mixed melt, kept at a constant temperature for 30 minutes, and then rapidly cooled to the saturation temperature of 315°C.

[0049] The temperature is then gradually decreased at a rate of 3°C / day, the seed crystal crucible is rotated at a rotation speed of 5 rpm, and after the crystal has grown to the required size, the crystal is lifted from the surface of the melt and cooled to room temperature at a rate of 1°C / h. The crystal is then removed from the hearth and placed in an A3B molten metal tube with a size of 25mm x 24mm x 10mm. 11 P2O 23 (A=K, Rb, Cs, NH4) crystals were obtained.

[0050] Example 4

[0051] Reaction formula: 3A2O (A = K, Rb, Cs, NH4) + 22H3BO3 + 2P2O5 → 2A3B 11 P2O 23 (A=K, Rb, Cs, NH4)+33H2O↑, 2A3B 11 P2O 23 (A=K, Rb, Cs, NH4) compounds were synthesized.

[0052] The raw materials a, A2CO3 (A = K, Rb, Cs, NH4), H3BO3, and NH4H2PO4 were weighed directly in a molar ratio of 3:22:2 and added to the polytetrafluoroethylene lining of an autoclave with a volume of 21 mL, and then 3 mL of deionized water was added and mixed thoroughly and uniformly to obtain a mixed solution.

[0053] b. The polytetrafluoroethylene-lined lid containing the mixture from step a was tightened and placed in a clean, contaminant-free autoclave, and the autoclave piston was tightened.

[0054] c) The autoclave in step b was placed in a thermostatic bath, heated to 120° C. at a heating rate of 20° C. / h, kept at the same temperature for 5 days, and then cooled to room temperature at a cooling rate of 4° C. / h.

[0055] d. The autoclave was opened, and the solution containing the crystals was filtered to obtain a series of alkali metal borophosphate compounds, and the obtained products were transparent crystals.

[0056] Example 5

[0057] Reaction formula: 3AF (A = K, Rb, Cs, NH4) + 11H3BO3 + 2NH4H2PO4 → A3B 11 P2O 23 According to (A=K, Rb, Cs, NH4)+18H2O↑+3HF↑+2NH3↑, A3B 11 P2O 23 (A=K, Rb, Cs, NH4) compounds were synthesized.

[0058] The raw materials a, AF (A = K, Rb, Cs, NH4), H3BO3, and NH4H2PO4 were directly weighed in a molar ratio of 3:11:2 and added to the polytetrafluoroethylene lining of an autoclave with a volume of 150 mL, and then 50 mL of deionized water was added and mixed thoroughly and uniformly to obtain a mixed solution.

[0059] b. The polytetrafluoroethylene-lined lid containing the mixture from step a was tightened and placed in a clean, contaminant-free autoclave, and the autoclave piston was tightened.

[0060] c. The autoclave in step 5 was placed in a thermostatic chamber, heated to 330° C. at a heating rate of 10° C. / h, kept at the same temperature for 10 days, and then cooled to room temperature at a heating rate of 3° C. / h.

[0061] d. The autoclave was opened, and the solution containing the crystals was filtered to obtain a series of alkali metal borophosphate compounds, and the obtained products were transparent crystals.

[0062] Example 6

[0063] Reaction formula: 3A2CO3 (A = K, Rb, Cs, NH4) + 11B2O3 + 4NH4H2PO4 → 2A3B 11 P2O 23 According to (A=K, Rb, Cs, NH4)+6H2O↑+3CO2↑+4NH3↑, A3B 11 P2O 23 (A=K, Rb, Cs, NH4) compounds were synthesized.

[0064] The raw materials A2CO3 (A=K, Rb, Cs, NH4), B2O3, and NH4H2PO4 were directly weighed in a molar ratio of 3:11:4 and added to a beaker with a volume of 10 mL, and 0.1 mL of deionized water was added and stirred until the solution became clear. The beaker was then placed on a heating table and kept at 25°C. After two days, the series of alkali metal borophosphate nonlinear optical crystals were obtained. To further grow it, a seed crystal of the series of crystals was suspended in the solution with a thin platinum wire. To reduce the evaporation of water, the beaker was covered with a polyethylene sheet and several tens of millimeter-sized holes were drilled on it. After three weeks, a series of centimeter-sized alkali metal borophosphate nonlinear optical crystals were taken out of the solution.

[0065] Example 7

[0066] Reaction formula: 3A2CO3 (A = K, Rb, Cs, NH4) + 11B2O3 + 2P2O5 → 2A3B 11 P2O 23 (A=K, Rb, Cs, NH4)+3CO2↑, A3B 11 P2O 23 (A=K, Rb, Cs, NH4) compounds were synthesized.

[0067] The raw materials A2CO3 (A=K, Rb, Cs, NH4), B2O3, and P2O5 were directly weighed in a molar ratio of 3:11:2 and added to a beaker with a volume of 1000 mL, and 400 mL of deionized water was added and stirred until the solution became transparent. Then, the beaker was placed on a heating table and heated to 400°C, and after 7 days, the series of alkali metal borophosphate nonlinear optical crystals were obtained. To further grow it, the seed crystals of the series of crystals were suspended in the solution with a thin platinum wire. To reduce the evaporation of water, the beaker was covered with a polyethylene sheet and tens of millimeter-sized holes were drilled on it. After 5 weeks, the series of alkali metal borophosphate nonlinear optical crystals with centimeter sizes were taken out of the solution.

[0068] Example 8

[0069] Reaction formula: 3AH2PO4 (A = K, Rb, Cs, NH4) + 5.5B2O3 → A3B11 P2O 23 According to (A=K, Rb, Cs, NH4) + 1.5H2O↑ + H3PO4, A3B 11 P2O 23 (A=K, Rb, Cs, NH4) compounds were synthesized.

[0070] The raw materials AH2PO4 (A=K, Rb, Cs, NH4) and B2O3 were directly weighed out in a molar ratio of 3:5.5, and the weighed raw materials were mixed with flux AOH (A=K, Rb, Cs, NH4)-PbO in a molar ratio of 4:7, where the molar ratio of AOH (A=K, Rb, Cs, NH4) to PbO was 1:6. The materials were placed in an open platinum crucible of Φ80mm×80mm, heated to 350℃, and kept at a constant temperature for 60 hours to obtain a mixed molten liquid, which was then cooled to 330℃.

[0071] The temperature was gradually lowered to room temperature at a rate of 3.5°C / h, and spontaneous crystallization occurred to obtain a series of alkali metal borophosphate seed crystals.

[0072] The obtained A3B 11 P2O 23 (A=K, Rb, Cs, NH4) A seed crystal was fixed to a seed crystal rod, lowered from the top of a crystal growth furnace, preheated on the surface of the mixed melt for 15 minutes, and then immersed below the liquid surface to melt back into the mixed melt, kept at a constant temperature for 30 minutes, and then rapidly cooled to the saturation temperature of 315°C.

[0073] The temperature was then gradually decreased at a rate of 3°C / day, and the seed crystal crucible was rotated at a rotation speed of 5 rpm. After the crystal had grown to the required size, the crystal was lifted from the surface of the melt and cooled to room temperature at a rate of 1°C / h. The crystal was then removed from the hearth and placed in a A3B 1000-mm diameter tube with a size of 25 mm x 24 mm x 10 mm. 11 P2O 23 (A=K, Rb, Cs, NH4) crystals were obtained.

[0074] Example 9

[0075] Reaction formula: 3A2HPO4 (A = K, Rb, Cs, NH4) + 11B2O3 + 0.5P2O5 → 2A3B11 P2O 23 (A=K, Rb, Cs, NH4)+1.5H2O↑, A3B 11 P2O 23 (A=K, Rb, Cs, NH4) compounds were synthesized.

[0076] The raw materials A2HPO4 (A=K, Rb, Cs, NH4), B2O3, and P2O5 were directly weighed out in a molar ratio of 3:11:0.5, and the weighed raw materials were mixed with the flux A2CO3 (A=K, Rb, Cs, NH4)-H3BO3-NH4H2PO4 in a molar ratio of 5:2, where the molar ratio of A2CO3 (A=K, Rb, Cs, NH4), H3BO3, and NH4H2PO4 was 5:16:16. The raw materials were placed in an open platinum crucible of Φ80mm×80mm, heated to 550℃, and kept at a constant temperature for 60 hours to obtain a mixed molten liquid, which was then cooled to 530℃.

[0077] The temperature was gradually lowered to room temperature at a rate of 3.5°C / h, and spontaneous crystallization occurred to obtain a series of alkali metal borophosphate seed crystals.

[0078] The obtained A3B 11 P2O 23 (A=K, Rb, Cs, NH4) A seed crystal was fixed to a seed crystal rod, lowered from the top of a crystal growth furnace, preheated on the surface of the mixed melt for 15 minutes, and then immersed below the liquid surface to melt back into the mixed melt, kept at a constant temperature for 30 minutes, and then rapidly cooled to the saturation temperature of 515°C.

[0079] The temperature was then gradually decreased at a rate of 3°C / day, and the seed crystal crucible was rotated at a rotation speed of 5 rpm. After the crystal had grown to the required size, the crystal was lifted from the surface of the melt and cooled to room temperature at a rate of 1°C / h. The crystal was then removed from the hearth and placed in a A3B 1000-mm diameter tube with a size of 25 mm x 24 mm x 10 mm. 11 P2O 23 (A=K, Rb, Cs, NH4) crystals were obtained.

[0080] Example 10

[0081] Reaction formula: 6AOH (A = K, Rb, Cs, NH4) + 11B2O3 + 2P2O5 → 2A3B 11 P2O 23 (A=K, Rb, Cs, NH4)+3H2O↑, A3B 11 P2O 23 (A=K, Rb, Cs, NH4) compounds were synthesized.

[0082] The raw materials AOH (A = K, Rb, Cs, NH4), B2O3, and P2O5 were directly weighed out in a molar ratio of 6:11:2, and the weighed raw materials were mixed with flux ABF4 (A = K, Rb, Cs, NH4)-MoO3 in a molar ratio of 9:3, where the molar ratio of H3BO3 and P2O5 was 4:7. The mixture was placed in an open platinum crucible with a diameter of 80 mm x 80 mm, heated to 450°C, and kept at a constant temperature for 60 hours to obtain a mixed molten liquid, which was then cooled to 400°C.

[0083] The temperature was gradually lowered to room temperature at a rate of 3.5°C / h, and spontaneous crystallization occurred to obtain a series of alkali metal borophosphate seed crystals.

[0084] The obtained A3B 11 P2O 23 (A=K, Rb, Cs, NH4) A seed crystal was fixed to a seed crystal rod, lowered from the top of a crystal growth furnace, preheated on the surface of the mixed melt for 15 minutes, and then immersed below the liquid surface to melt back into the mixed melt, kept at a constant temperature for 30 minutes, and then rapidly cooled to the saturation temperature of 405°C.

[0085] The temperature is then gradually decreased at a rate of 3°C / day, the seed crystal crucible is rotated at a rotation speed of 5 rpm, and after the crystal has grown to the required size, the crystal is lifted from the surface of the melt and cooled to room temperature at a rate of 1°C / h. The crystal is then removed from the hearth and placed in an A3B molten metal tube with a size of 25mm x 24mm x 10mm. 11 P2O 23 (A=K, Rb, Cs, NH4) crystals were obtained.

[0086] Example 11

[0087] Reaction formula: 12AH2PO4 (A = K, Rb, Cs, NH4) + 22H3B2O3 + 2P2O5 → 4A3B 11 P2O 23 (A=K, Rb, Cs, NH4) + 33H2↑ + 8H3PO4, 2A3B 11 P2O 23 (A=K, Rb, Cs, NH4) compounds were synthesized.

[0088] The raw materials a, AH2PO4 (A = K, Rb, Cs, NH4), H3BO3, and P2O5 were weighed directly in a molar ratio of 12:22:2 and added to the polytetrafluoroethylene lining of an autoclave with a volume of 100 mL. 50 g of boric acid was then added and mixed thoroughly and uniformly to obtain a mixed liquid.

[0089] b. The polytetrafluoroethylene-lined lid containing the mixture from step a was tightened and placed in a clean, contaminant-free autoclave, and the autoclave piston was tightened.

[0090] c) The autoclave from step b was placed in a thermostatic bath, heated to 180° C. at a heating rate of 20° C. / h, kept at the same temperature for 10 days, and then cooled to room temperature at a cooling rate of 4° C. / h.

[0091] d. The autoclave was opened, and the solution containing the crystals was filtered to obtain a series of alkali metal borophosphate compounds, and the obtained products were transparent crystals.

[0092] Example 12

[0093] Reaction formula: 6ACl (A = K, Rb, Cs, NH4) + 11B2O3 + 4NH4H2PO4 → 2A3B 11 P2O 23 According to (A=K, Rb, Cs, NH4)+6HCl↑+4NH3↑+3H2O↑, A3B 11 P2O 23 (A=K, Rb, Cs, NH4) compounds were synthesized.

[0094] The raw materials a, ACl (A = K, Rb, Cs, NH4), B2O3, and NH4H2PO4 were weighed directly in a molar ratio of 6:11:4 and added to the polytetrafluoroethylene lining of an autoclave with a volume of 21 mL, and 0.1 g of phosphoric acid was further added and mixed thoroughly and uniformly to obtain a mixed solution.

[0095] b. The polytetrafluoroethylene-lined lid containing the mixture from step a was tightened and placed in a clean, contaminant-free autoclave, and the autoclave piston was tightened.

[0096] c) The autoclave from step b was placed in a thermostatic bath, heated to 160° C. at a heating rate of 10° C. / h, kept at the same temperature for 11 days, and then cooled to room temperature at a cooling rate of 4° C. / h.

[0097] d. The autoclave was opened, and the solution containing the crystals was filtered to obtain a series of alkali metal borophosphate compounds, and the obtained products were transparent crystals.

[0098] Example 13

[0099] Reaction formula: 6ACl (A = K, Rb, Cs, NH4) + 22H3BO3 + 2P2O5 → 2A3B 11 P2O 23 According to (A=K, Rb, Cs, NH4) + 6HCl↑ + 30H2O↑, A3B 11 P2O 23 (A=K, Rb, Cs, NH4) compounds were synthesized.

[0100] The raw materials ACl (A=K, Rb, Cs, NH4), H3BO3, and P2O5 were directly weighed in a molar ratio of 6:22:2 and added to a beaker with a volume of 10 mL, and 0.1 mL of deionized water was added and stirred until the solution became transparent. The beaker was then placed on a heating table and heated to 400°C, and after 7 days, the series of alkali metal borophosphate nonlinear optical crystals were obtained. To further grow it, a seed crystal of the series of crystals was suspended in the solution with a thin platinum wire. To reduce the evaporation of water, the beaker was covered with a polyethylene sheet and several tens of millimeter-sized holes were drilled on it. After 5 weeks, a series of centimeter-sized alkali metal borophosphate nonlinear optical crystals were taken out of the solution.

[0101] Example 14

[0102] Any of the K3Bs obtained in Examples 1 to 13 11 P2O 23 , Rb3B 11 P2O 23 , Cs3B 11 P2O 23 or (NH4)3B 11 P2O 23 The crystal was processed into a single crystal device according to the alignment direction and placed at position 3 as shown in Figure 4. At room temperature, a Nd:YAG Q-switched laser source with a wavelength of 1064 nm was used as the pump source, and the K3B 11 P2O 23 , Rb3B 11 P2O 23 , Cs3B 11 P2O 23 or (NH4)3B 11 P2O 23 The light is incident on a nonlinear optical crystal 3 to generate frequency-doubled light with a wavelength of 532 nm. The output beam 4 contains infrared light with a wavelength of 1064 nm and frequency-doubled light with a wavelength of 532 nm. After filtering through a filter 5, a laser light with a wavelength of 532 nm is obtained.

[0103] Example 15

[0104] Any of the K3Bs obtained in Examples 1 to 13 11 P2O 23 , Rb3B11 P2O 23 , Cs3B 11 P2O 23 or (NH4)3B 11 P2O 23 The crystal was processed into a single crystal device according to the alignment direction and placed at position 3 as shown in Figure 4. At room temperature, a Nd:YAG Q-switched laser source with a wavelength of 532 nm was used as the pump source, and the K3B 11 P2O 23 , Rb3B 11 P2O 23 , Cs3B 11 P2O 23 or (NH4)3B 11 P2O 23 The light is incident on a nonlinear optical crystal 3 to generate frequency-doubled light with a wavelength of 266 nm. The output beam 4 contains frequency-doubled light with wavelengths of 532 nm and 266 nm, and after filtering through a filter 5, a laser beam with a wavelength of 266 nm is obtained.

[0105] Example 16

[0106] Any of the K3Bs obtained in Examples 1 to 13 11 P2O 23 , Rb3B 11 P2O 23 , Cs3B 11 P2O 23 or (NH4)3B 11 P2O 23 The crystals were fabricated into single crystal devices via directional cutting and polishing processes and pumped with a 1064 nm Nd:YAG Q-switched laser source to generate laser output with a wavelength of less than 266 nm.

Claims

1. A borophosphate compound, the molecular formula of which is A 3 B 11 P 2 O 23 where A=K, Rb, Cs, NH 4 and the molecular formula is K 3 B 11 P 2 O 23 , Rb 3 B 11 P 2 O 23 , Cs 3 B 11 P 2 O 23 or (NH 4 ) 3 B 11 P 2 O 23 and the molecular weights are 666.15, 805.26, 947.57 and 602.97, respectively.

2. A using a solid-state reaction method 3 B 11 P 2 O 23 Prepare a compound represented by the formula: 4 The specific operation of the compound is as follows: A = K, Rb, Cs, NH 4 The boron-containing compound, the boron-containing compound, and the phosphorus-containing compound are uniformly mixed and crushed, and then placed in a muffle furnace for firing, and a single-phase polycrystalline powder of borophosphate compound is prepared through multiple grinding and firing processes, where A=K, Rb, Cs, NH 4 the molar ratio of element A in the containing compound, element boron in the boron-containing compound, and element phosphorus in the phosphorus-containing compound is 2.5-3.5:10.5-11.5:1.5-2.5; Said A=K, Rb, Cs, NH 4 The compounds contained are AOH, A 2 O, and at least one of alkali metal salts, the alkali metal salts being AF, AC1, ABr, and ANO 3 , A 2 C 2 O 4 , A 2 CO 3 , A.H.C.O. 3 , A 2 SO 4 where A=K, Rb, Cs, NH 4 and The boron-containing compound is B 2 O 3 , H 3 B.O. 3 and a borate, the borate being selected from the group consisting of ABO 2 , A.B.O. 3 , A 3 B.O. 3 , A 2 B 4 O 7 where A=K, Rb, Cs, NH 4 and The phosphorus-containing compound is P 2 O 5 , H 3 P.O. 4 and a phosphate, the phosphate being AH 2 P.O. 4 , A 2 H.P.O. 4 , A 3 P.O. 4 , A 2 H 2 P 2 O 7 , A 4 P 2 O 7 where A=K, Rb, Cs, NH 4 2. A method for preparing a borophosphate compound, comprising the steps of:

3. A using a hydrothermal method 3 B 11 P 2 O 23 Prepare a compound represented by the formula: 4 The specific operation of the compound is as follows: A = K, Rb, Cs, NH 4The boron-containing compound, the boron-containing compound and the phosphorus-containing compound are added to the polytetrafluoroethylene lining of the autoclave, and then deionized water and a mineralizer are added and mixed thoroughly and uniformly to obtain a mixture, where A=K, Rb, Cs, NH 4 the molar ratio of the powder-containing compound, the boron-containing compound, and the phosphorus-containing compound is 1-4:10-12:1-3; the polytetrafluoroethylene lining is placed in an autoclave, the autoclave is placed in a thermostatic bath, heated, and kept at a constant temperature for a certain period of time, and then cooled to lower the temperature; and the solution containing the powder is filtered to obtain the borophosphate compound; Said A=K, Rb, Cs, NH 4 The compounds contained are AOH, A 2 O, and at least one of alkali metal salts, the alkali metal salts being AF, AC1, ABr, and ANO 3 , A 2 C 2 O 4 , A 2 CO 3 , A.H.C.O. 3 , A 2 SO 4 where A=K, Rb, Cs, NH 4 and The boron-containing compound is B 2 O 3 , H 3 B.O. 3 and a borate, the borate being selected from the group consisting of ABO 2 , A.B.O. 3 , A 3 B.O. 3 , A 2 B 4 O 7 where A=K, Rb, Cs, NH 4 and The phosphorus-containing compound is P 2 O 5 , H 3 P.O. 4 and a phosphate, the phosphate being AH 2 P.O. 4 , A 2 H.P.O. 4 , A 3 P.O. 4 , A 2 H 2 P 2 O 7 , A 4 P 2 O 7 where A=K, Rb, Cs, NH 4 2. A method for preparing a borophosphate compound, comprising the steps of:

4. A borophosphate nonlinear optical crystal, the chemical formula of the crystal being A 3 B 11 P 2 O 23 (A=K, Rb, Cs, NH 4 ) and the molecular formula is K 3 B 11 P 2 O 23 , Rb 3 B 11 P 2 O 23 , Cs 3 B 11 P 2 O 23 or (NH 4 ) 3 B 11 P 2 O 23 Both crystallize in the trigonal system in the space group R3, with unit cell parameters of [Case 2] , α=90°, β=90°, γ=120°, and Z=3.

5. A using a high-temperature melt method 3 B 11 P 2 O 23 where A=K, Rb, Cs, NH 4 The specific operation of the nonlinear optical crystal is a single-phase polycrystalline powder of a borophosphate compound, or a mixture of a single-phase polycrystalline powder of a borophosphate compound and a flux, or directly A=K, Rb, Cs, NH 4A = K, Rb, Cs, NH 4 the mixture of the boron-containing compound, the boron-containing compound, the phosphorus-containing compound and the flux is heated until melted to obtain a mixed melt; then the crucible containing the mixed melt is placed in a crystal growth furnace and heated, and cooled to a saturation temperature; at this time, a seed crystal rod is inserted below the liquid surface; and then the seed crystal rod is pulled out from the liquid surface before the melt solidifies, thereby preparing a borophosphate nonlinear optical crystal; The molar ratio of the single-phase polycrystalline powder of the borophosphate compound to the flux is 1:0-20; or A=K, Rb, Cs, NH 4 The method for preparing borophosphate nonlinear optical crystal according to claim 4, characterized in that the molar ratio of the containing compound, the boron containing compound, the phosphorus containing compound and the flux is 2.5-3.5:10.5-11.5:1.5-2.5:0-20, wherein the flux comprises alkali metal salts, namely alkali metal carbonates, alkali metal nitrates, alkali metal sulfates, alkali metal oxalates, alkali metal borates, alkali metal phosphates, alkali metal halides, alkali metal fluoroborates, alkali metal metaborates, and alkali metal oxides, alkali metal hydroxides, and at least one of monohydrogen phosphates, dihydrogen phosphates, boron oxides, boric acid, phosphoric acid, lead oxides, lead fluorides, molybdenum oxides, and bismuth oxides.

6. A using a hydrothermal method 3 B 11 P 2 O 23 where A=K, Rb, Cs, NH 4 The specific operation of the nonlinear optical crystal is a single-phase polycrystalline powder of a borophosphate compound, or a mixture of a single-phase polycrystalline powder of a borophosphate compound and a mineralizer, or directly A=K, Rb, Cs, NH 4 A = K, Rb, Cs, NH 4the mixture of the boron-containing compound, the boron-containing compound and the phosphorus-containing compound and the mineralizer is added to the polytetrafluoroethylene lining of the autoclave, deionized water is further added, and the mixture is thoroughly mixed uniformly to obtain a mixture, the polytetrafluoroethylene lining is placed in the autoclave, the autoclave is placed in a thermostatic bath to heat, and then cooled to room temperature, and the solution containing the crystals is filtered to obtain a transparent borophosphate nonlinear optical crystal; The molar ratio of the single-phase polycrystalline powder of the borophosphate compound to the mineralizer is 1:0-10; or A=K, Rb, Cs, NH 4 The molar ratio of the mineralizer to the boron-containing compound, the boron-containing compound and the phosphorus-containing compound is 2-4:10-12:1-3:0-10, and the mineralizer is AOH, A 2 O, AF, ACl, ABr, ABF 4 , A 3 P.O. 4 , A 3 B.O. 3 , A.N.O. 3 , A 2 C 2 O 4 , A 2 CO 3 , A.H.C.O. 3 , A 2 SO 4 , A 2 H.P.O. 4 , A.H. 2 P.O. 4 , B 2 O 3 5. The method for preparing a borophosphate nonlinear optical crystal according to claim 4, characterized in that it comprises at least one or more of the following:

7. A using a solution method 3 B 11 P 2 O 23 where A=K, Rb, Cs, NH 4 The specific operation of the nonlinear optical crystal is a single-phase polycrystalline powder of a borophosphate compound or a mixture of a single-phase polycrystalline powder of a borophosphate compound and a cosolvent, or directly A=K, Rb, Cs, NH 4A = K, Rb, Cs, NH 4 adding the mixture of the containing compound, the boron containing compound and the phosphorus containing compound and the co-solvent to a beaker, adding deionized water to dissolve, stirring the solution until it becomes clear, and then placing the beaker in air to evaporate the solution to grow a borophosphate nonlinear optical crystal; The molar ratio of the single-phase polycrystalline powder of the borophosphate compound to the co-solvent is 1:0-30, or A=K, Rb, Cs, NH 4 The method for preparing borophosphate nonlinear optical crystal according to claim 4, characterized in that the molar ratio of the containing compound, the boron containing compound and the phosphorus containing compound to the co-solvent is 2.5-3.5:10.5-11.5:1.5-2.5:0-30, and the co-solvent is a self-co-solvent.

8. 1. A nonlinear optical device comprising: an apparatus for passing at least one incident electromagnetic radiation through at least one nonlinear optical crystal to produce output radiation having at least one frequency different from the incident electromagnetic radiation, the nonlinear optical crystal being a borophosphate nonlinear optical crystal A. 3 B 11 P 2 O 23 where A=K, Rb, Cs, NH 4 A nonlinear optical device comprising:

9. A method for using the borophosphate nonlinear optical crystal described in claim 4, characterized in that the borophosphate nonlinear optical crystal is used in a second harmonic generator, an up-down frequency converter, an optical parametric oscillator, a laser frequency conversion device, or a nonlinear optical device for laser communications.

Citation Information

Patent Citations

  • Compound rubidium-boron-phosphorus-oxygen, rubidium-boron-phosphorus-oxygen nonlinear optical crystal as well as preparation method and application thereof