Semiconductor Device
The semiconductor device addresses adhesion and breakdown voltage issues by incorporating a barrier height adjustment region and guard ring, enhancing Schottky characteristics and breakdown voltage for improved thermal stability and reduced forward voltage rise.
Patent Information
- Application Number
- JP2023050423
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2017-07-08
- Filing Date
- 2023-03-27
- Publication Date
- 2024-12-09
- Estimated Expiration
- 2038-07-06
AI Technical Summary
Conventional semiconductor devices with Schottky barrier electrodes face issues with adhesion at junctions, temperature-dependent barrier height changes, and inadequate breakdown voltage, particularly when guard rings are short-circuited, leading to deteriorated withstand voltage.
The semiconductor device incorporates a barrier height adjustment region with a higher barrier height than the interface between the semiconductor region and the barrier electrode, embedded or protruding into the semiconductor region, and optionally includes a guard ring at the outer periphery, using materials like metal oxides and metals to enhance adhesion and reduce electric field concentration.
The solution results in improved Schottky characteristics, enhanced temperature stability, reduced forward voltage rise, and increased breakdown voltage, while maintaining excellent thermal stability and adhesion, making it suitable for power devices.
Smart Images

Figure 0007595966000001 
Figure 0007595966000002 
Figure 0007595966000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a semiconductor device useful as a power device or the like, and a semiconductor system including the same. [Background technology]
[0002] Conventionally, semiconductor devices having a Schottky barrier electrode provided on a semiconductor substrate have been known, and various studies have been conducted on the Schottky barrier electrode with the aim of increasing the reverse breakdown voltage and further decreasing the forward rise voltage. Patent Document 1 describes a method of increasing the reverse breakdown voltage and decreasing the forward rise voltage by arranging a metal with a small barrier height in the center of a semiconductor and forming a Schottky contact between a metal with a large barrier height and a semiconductor in the peripheral part of the semiconductor.
[0003] In addition, the combination of a Schottky electrode and an ohmic electrode has also been studied. For example, Patent Document 2 describes a wide band gap semiconductor device in which a Schottky electrode and an ohmic electrode made of the same metal are formed on a substrate, and it is described that such a configuration can improve thermal breakdown resistance when a high current such as a surge current flows in the forward direction. However, there are problems with the adhesion of the interfaces between the Schottky junction and the ohmic junction and the adhesion between the junctions, and the electrode material needs to be limited. Furthermore, there is a problem that the barrier height changes depending on the temperature, and the results are not necessarily satisfactory. Therefore, a semiconductor device with a low start-up voltage and excellent temperature stability has been awaited.
[0004] In addition, Patent Document 3 describes a semiconductor device in which a conductive guard ring and a main junction joined to a Schottky electrode are connected via a short circuit, and describes that such a semiconductor device reduces electric field concentration and contributes to improving the breakdown voltage. However, even if many guard rings are installed, there is a problem that the breakdown voltage is deteriorated because they are short-circuited with the main junction. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 52-101970 [Patent Document 2] JP 2014-78660 A [Patent Document 3] JP 2014-107408 A Summary of the Invention [Problem to be solved by the invention]
[0006] An object of the present invention is to provide a semiconductor device having excellent Schottky characteristics and semiconductor characteristics. [Means for solving the problem]
[0007] As a result of intensive research into achieving the above-mentioned object, the inventors have discovered that in a semiconductor device comprising at least a semiconductor region and a barrier electrode provided on the semiconductor region, by embedding, on the surface of the semiconductor region between the semiconductor region and the barrier electrode, a plurality of barrier height adjusting regions in which the barrier height with the barrier electrode is greater than the barrier height at the interface between the semiconductor region and the barrier electrode, it is possible to lower the start-up voltage, improve the temperature stability, and further improve the breakdown voltage, and have found that such a semiconductor device can solve the above-mentioned conventional problems in one fell swoop. After obtaining the above findings, the inventors conducted further studies and completed the present invention.
[0008] That is, the present invention relates to the following inventions. [1] A semiconductor device comprising at least a semiconductor region and a barrier electrode provided on the semiconductor region, characterized in that a barrier height adjusting region is provided between the semiconductor region and the barrier electrode, in which the barrier height at the interface between the semiconductor region and the barrier electrode is greater than the barrier height at the interface between the semiconductor region and the barrier electrode, and the barrier height adjusting region is provided in plurality on the surface of the semiconductor region. [2] A semiconductor device comprising at least a semiconductor region and a barrier electrode provided on the semiconductor region, wherein a barrier height adjusting region is provided between the semiconductor region and the barrier electrode, in which the barrier height at the interface between the semiconductor region and the barrier electrode is greater than the barrier height at the interface between the semiconductor region and the barrier electrode, and the barrier height adjusting region is embedded in a surface of the semiconductor region in plurality. [3] The semiconductor device according to [1], wherein the barrier height adjusting regions are provided between both ends of the barrier electrode and the semiconductor region. [4] The semiconductor device according to [1], wherein the barrier height adjusting region protrudes into the barrier electrode. [5] The semiconductor device according to [1], wherein a guard ring is provided around the outer periphery of the barrier electrode. [6] The semiconductor device according to [5], wherein a part or all of the guard ring is embedded in the surface of the semiconductor region. [7] The semiconductor device according to [1], wherein a barrier height at an interface between the barrier electrode and the barrier height adjusting region is 1 eV or more. [8] The semiconductor device according to [1], wherein the barrier electrode is made of a metal. [9] The semiconductor device according to [1], wherein the semiconductor region contains a crystalline oxide semiconductor as a main component.
[10] The semiconductor device according to [1], wherein the semiconductor region contains a gallium compound as a main component.
[11] The semiconductor device according to [1], wherein the semiconductor region contains α-Ga2O3 or an alloy thereof as a main component.
[12] The semiconductor device according to [1] or [2], wherein the barrier height adjusting region contains a p-type oxide semiconductor as a main component.
[13] The semiconductor device according to [1] or [2], wherein the barrier height adjusting region contains, as a main component, a p-type oxide semiconductor having a corundum structure or a hexagonal structure.
[14] The semiconductor device according to [1], which is a diode.
[15] The semiconductor device according to [1], which is a junction barrier Schottky diode.
[16] The semiconductor device according to [1] above, which is a power device.
[17] A semiconductor system including a semiconductor device, the semiconductor device being the semiconductor device according to any one of [1] to
[16] above. Effect of the Invention
[0009] The semiconductor device of the present invention has excellent Schottky characteristics and semiconductor characteristics. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 is a diagram showing a schematic diagram of a preferred embodiment of a junction barrier Schottky diode (JBS) of the present invention. [Diagram 2] 2A to 2C are diagrams illustrating a preferred method for manufacturing the junction barrier Schottky diode (JBS) of FIG. 1. [Diagram 3] FIG. 1 is a diagram showing a schematic diagram of a preferred embodiment of a junction barrier Schottky diode (JBS) of the present invention. [Figure 4] 4A to 4C are diagrams illustrating a preferred method for manufacturing the junction barrier Schottky diode (JBS) of FIG. 3. [Diagram 5] 4A to 4C are diagrams illustrating a preferred method for manufacturing the junction barrier Schottky diode (JBS) of FIG. 3. [Figure 6]FIG. 1 is a diagram illustrating a preferred example of a power supply system. [Figure 7] FIG. 1 is a diagram illustrating a preferred example of a system device. [Figure 8] FIG. 1 is a diagram illustrating a preferred example of a power supply circuit diagram of a power supply device. [Figure 9] FIG. 1 is a schematic diagram of a film forming apparatus (mist CVD apparatus) used in a reference example. [Figure 10] FIG. 13 shows IV measurement results in a reference example, where (a) shows the forward measurement result and (b) shows the reverse measurement result. [Figure 11] FIG. 1 is a diagram showing a schematic diagram of a preferred embodiment of a junction barrier Schottky diode (JBS) of the present invention. [Figure 12] 12A to 12C are diagrams illustrating a preferred method for manufacturing the junction barrier Schottky diode (JBS) of FIG. 11. [Figure 13] FIG. 1 is a diagram showing a schematic diagram of a preferred embodiment of a junction barrier Schottky diode (JBS) of the present invention. [Figure 14] 14A to 14C are diagrams illustrating a preferred method for manufacturing the junction barrier Schottky diode (JBS) of FIG. 13. [Figure 15] FIG. 1 is a diagram showing a schematic diagram of a preferred embodiment of a junction barrier Schottky diode (JBS) of the present invention. [Figure 16] FIG. 1 is a diagram showing a schematic diagram of a preferred embodiment of a junction barrier Schottky diode (JBS) of the present invention. [Figure 17] FIG. 1 is a diagram showing a schematic diagram of a preferred embodiment of a junction barrier Schottky diode (JBS) of the present invention. [Figure 18] FIG. 1 is a diagram showing a schematic diagram of a preferred embodiment of a junction barrier Schottky diode (JBS) of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The semiconductor device of the present invention is a semiconductor device comprising at least a semiconductor region and a barrier electrode provided on the semiconductor region, and is characterized in that a barrier height adjusting region is provided between the semiconductor region and the barrier electrode, in which the barrier height at the interface between the semiconductor region and the barrier electrode is greater than the barrier height at the interface between the semiconductor region and the barrier electrode, and the barrier height adjusting region is provided in plurality on the surface of the semiconductor region. The semiconductor device of the present invention is characterized in that it comprises at least a semiconductor region and a barrier electrode provided on the semiconductor region, and a barrier height adjusting region is provided between the semiconductor region and the barrier electrode, in which the barrier height at the interface between the semiconductor region and the barrier electrode is greater than the barrier height at the interface between the semiconductor region and the barrier electrode, and a plurality of the barrier height adjusting regions are embedded in the surface of the semiconductor region. In the present invention, it is also preferable that the barrier height adjusting region protrudes into the barrier electrode, and it is more preferable that the barrier height adjusting region is embedded in the surface of the semiconductor region and protrudes into the barrier electrode. According to the above-mentioned preferred embodiment, it is possible to further suppress electric field concentration and further reduce contact resistance.
[0012] The barrier electrode is not particularly limited as long as it forms a Schottky barrier having a predetermined barrier height at the interface with the semiconductor region. The electrode material of the barrier electrode is not particularly limited as long as it can be used as a barrier electrode, and may be a conductive inorganic material or a conductive organic material. In the present invention, the electrode material is preferably a metal. The metal is not particularly limited, but preferably includes at least one metal selected from Groups 4 to 11 of the periodic table. Examples of metals in Group 4 of the periodic table include titanium (Ti), zirconium (Zr), and hafnium (Hf), among which Ti is preferred. Examples of metals in Group 5 of the periodic table include vanadium (V), niobium (Nb), and tantalum (Ta). Examples of metals in Group 6 of the periodic table include one or more metals selected from chromium (Cr), molybdenum (Mo), and tungsten (W), but in the present invention, Cr is preferred because it provides better semiconductor properties such as switching properties. Examples of metals in Group 7 of the periodic table include manganese (Mn), technetium (Tc), and rhenium (Re). Examples of metals in Group 8 of the periodic table include iron (Fe), ruthenium (Ru), and osmium (Os). Examples of metals in Group 9 of the periodic table include cobalt (Co), rhodium (Rh), and iridium (Ir). Examples of metals in Group 10 of the periodic table include nickel (Ni), palladium (Pd), and platinum (Pt), with Pt being preferred. Examples of metals in Group 11 of the periodic table include copper (Cu), silver (Ag), and gold (Au). Examples of the means for forming the barrier electrode include known means, and more specifically, examples of the means include dry methods and wet methods. Examples of dry methods include known means such as sputtering, vacuum deposition, and CVD. Examples of wet methods include screen printing and die coating.
[0013] The semiconductor region is not particularly limited as long as it is mainly composed of a semiconductor, but in the present invention, the semiconductor region preferably contains a crystalline oxide semiconductor as a main component, and is more preferably an n-type semiconductor region mainly composed of an n-type semiconductor. The crystalline oxide semiconductor preferably has a β-gallium structure or a corundum structure, and more preferably has a corundum structure. The semiconductor region also preferably contains a gallium compound as a main component, more preferably an InAlGaO-based semiconductor as a main component, and most preferably contains α-Ga2O3 or a mixed crystal thereof as a main component. Note that the "main component" may mean, for example, when the crystalline oxide semiconductor is α-Ga2O3, that the atomic ratio of gallium in the metal elements in the semiconductor region is 0.5 or more and α-Ga2O3 is contained. In the present invention, the atomic ratio of gallium in the metal elements in the semiconductor region is preferably 0.7 or more, and more preferably 0.8 or more. Furthermore, the semiconductor region is usually a single-phase region, but may further include a second semiconductor region made of a different semiconductor phase or other phases, so long as the object of the present invention is not hindered. Furthermore, the semiconductor region is usually in a film form, and may be a semiconductor film. The thickness of the semiconductor film in the semiconductor region is not particularly limited, and may be 1 μm or less, or 1 μm or more, but in the present invention, it is preferably 1 μm to 40 μm, and more preferably 1 μm to 25 μm. The surface area of the semiconductor film is not particularly limited, but is preferably 1 mm 2 May be more than 1mm 2The crystalline oxide semiconductor is usually single crystal, but may be polycrystalline. The semiconductor film may be a single layer film or a multilayer film. When the semiconductor film is a multilayer film, the multilayer film is preferably 40 μm or less in thickness. Also, when the semiconductor film is a multilayer film including at least a first semiconductor layer and a second semiconductor layer, and a Schottky electrode is provided on the first semiconductor layer, the multilayer film is preferably a multilayer film in which the carrier concentration of the first semiconductor layer is smaller than the carrier concentration of the second semiconductor layer. In this case, the second semiconductor layer usually contains a dopant, and the carrier concentration of the semiconductor layer can be appropriately set by adjusting the doping amount.
[0014] The semiconductor film preferably contains a dopant. The dopant is not particularly limited and may be a known one. Examples of the dopant include n-type dopants such as tin, germanium, silicon, titanium, zirconium, vanadium, or niobium, or p-type dopants. In the present invention, the dopant is preferably Sn, Ge, or Si. The content of the dopant in the composition of the semiconductor film is preferably 0.00001 atomic % or more, more preferably 0.00001 atomic % to 20 atomic %, and most preferably 0.00001 atomic % to 10 atomic %. In the present invention, it is preferable that the dopant used in the first semiconductor layer is germanium, silicon, titanium, zirconium, vanadium, or niobium, and the dopant used in the second semiconductor layer is tin, since the semiconductor properties are further improved without impairing the adhesion.
[0015] The semiconductor film is preferably formed by, for example, using a means such as a mist CVD method, and more specifically, for example, by atomizing or forming droplets from a raw material solution (atomization / dropletization process), transporting the obtained mist or droplets onto a substrate by a carrier gas (transportation process), and then causing a thermal reaction of the mist or droplets in a film formation chamber to laminate a semiconductor film containing a crystalline oxide semiconductor as a main component on the substrate (film formation process).
[0016] (Atomization / dropletization process) In the atomization / dropletization step, the raw solution is atomized or dropletized. The atomization means or dropletization means for the raw solution is not particularly limited as long as it can atomize or dropletize the raw solution, and may be a known means, but in the present invention, an atomization means or dropletization means using ultrasonic waves is preferred. The mist or droplets obtained using ultrasonic waves are preferable because they have an initial velocity of zero and float in the air, and are not sprayed like a spray, but are mist that floats in space and can be transported as a gas, so there is no damage due to collision energy, which is very suitable. The droplet size is not particularly limited, and may be droplets of about several mm, but is preferably 50 μm or less, and more preferably 100 nm to 10 μm.
[0017] (Raw material solution) The raw material solution is not particularly limited as long as it can be atomized or turned into droplets and contains a raw material capable of forming a semiconductor region, and may be an inorganic material or an organic material. However, in the present invention, the raw material is preferably a metal or a metal compound, and more preferably contains one or more metals selected from gallium, iron, indium, aluminum, vanadium, titanium, chromium, rhodium, nickel, cobalt, zinc, magnesium, calcium, silicon, yttrium, strontium, and barium.
[0018] In the present invention, the raw material solution can be suitably used in which the metal is dissolved or dispersed in an organic solvent or water in the form of a complex or salt. Examples of the complex include acetylacetonate complexes, carbonyl complexes, ammine complexes, and hydride complexes. Examples of the salt include organic metal salts (e.g., metal acetates, metal oxalates, and metal citrates), metal sulfides, metal nitrates, metal phosphates, and metal halides (e.g., metal chlorides, metal bromides, and metal iodides).
[0019] In addition, it is preferable to mix additives such as hydrohalogenated acid and oxidizing agents into the raw material solution. Examples of the hydrohalogenated acid include hydrobromic acid, hydrochloric acid, and hydroiodic acid, and among them, hydrobromic acid and hydroiodic acid are preferable because they can produce a better quality film. Examples of the oxidizing agent include peroxides such as hydrogen peroxide (H2O2), sodium peroxide (Na2O2), barium peroxide (BaO2), and benzoyl peroxide (C6H5CO)2O2, hypochlorous acid (HClO), perchloric acid, nitric acid, ozone water, and organic peroxides such as peracetic acid and nitrobenzene.
[0020] The raw material solution may contain a dopant. By adding a dopant to the raw material solution, doping can be performed well. The dopant is not particularly limited as long as it does not impede the object of the present invention. Examples of the dopant include n-type dopants such as tin, germanium, silicon, titanium, zirconium, vanadium, or niobium, and p-type dopants. The concentration of the dopant is usually about 1×10 16 / cm 3 ~1×10 22 / cm 3 Alternatively, the concentration of the dopant may be, for example, about 1×10 17 / cm 3 In accordance with the present invention, the dopant may be present in a concentration as low as about 1×10 20 / cm 3 In the present invention, the concentration of 1×10 17 / cm 3 It is preferable that the carrier concentration is equal to or higher than this.
[0021] The solvent of the raw material solution is not particularly limited, and may be an inorganic solvent such as water, an organic solvent such as alcohol, or a mixed solvent of an inorganic solvent and an organic solvent. In the present invention, the solvent preferably contains water, and more preferably is water or a mixed solvent of water and alcohol.
[0022] (Transportation process) In the transport step, the mist or droplets are transported into the film formation chamber by a carrier gas. The carrier gas is not particularly limited as long as it does not impede the object of the present invention, and suitable examples include inert gases such as oxygen, ozone, nitrogen, and argon, and reducing gases such as hydrogen gas and forming gas. The type of carrier gas may be one type, but may be two or more types, and a dilution gas with a reduced flow rate (for example, a 10-fold dilution gas, etc.) may be further used as a second carrier gas. The number of supply points of the carrier gas may be not only one but also two or more. The flow rate of the carrier gas is not particularly limited, but is preferably 0.01 to 20 L / min, and more preferably 1 to 10 L / min. In the case of a dilution gas, the flow rate of the dilution gas is preferably 0.001 to 2 L / min, and more preferably 0.1 to 1 L / min.
[0023] (Film forming process) In the film formation process, the mist or droplets are thermally reacted in a film formation chamber to form the semiconductor film on the substrate. The thermal reaction may be carried out at a temperature equal to or higher than the evaporation temperature of the solvent, and the reaction conditions are not particularly limited as long as the object of the present invention is not hindered. In this process, the thermal reaction is usually carried out at a temperature equal to or higher than the evaporation temperature of the solvent, but is preferably not too high (for example, 1000°C) or lower, more preferably 650°C or lower, and most preferably 300°C to 650°C. In addition, the thermal reaction may be carried out under any of vacuum, non-oxygen atmosphere, reducing gas atmosphere, and oxygen atmosphere as long as the object of the present invention is not hindered, but is preferably carried out under a non-oxygen atmosphere or oxygen atmosphere. In addition, the thermal reaction may be carried out under any of atmospheric pressure, pressurized, and reduced pressure conditions, but in the present invention, it is preferably carried out under atmospheric pressure. The film thickness can be set by adjusting the film formation time.
[0024] (Base) The substrate is not particularly limited as long as it can support the semiconductor film. The material of the substrate is not particularly limited as long as it does not impede the object of the present invention, and may be a known substrate, an organic compound, or an inorganic compound. The substrate may have any shape, and is effective for any shape, such as a plate shape such as a flat plate or a disk, a fiber shape, a rod shape, a column shape, a prism shape, a tube shape, a spiral shape, a sphere shape, a ring shape, etc., but in the present invention, a substrate is preferred. The thickness of the substrate is not particularly limited in the present invention.
[0025] The substrate is not particularly limited as long as it is plate-shaped and serves as a support for the semiconductor film. It may be an insulating substrate, a semiconductor substrate, a metal substrate, or a conductive substrate, but the substrate is preferably an insulating substrate, and is also preferably a substrate having a metal film on its surface. Examples of the substrate include a substrate containing a substrate material having a corundum structure as a main component, a substrate containing a substrate material having a β-gallium structure as a main component, and a substrate containing a substrate material having a hexagonal crystal structure as a main component. Here, the term "main component" means that the substrate material having the specific crystal structure is preferably contained in an atomic ratio of 50% or more, more preferably 70% or more, and even more preferably 90% or more of the total components of the substrate material, and may be 100%.
[0026] The substrate material is not particularly limited, and may be any known material, so long as it does not impede the object of the present invention. Suitable examples of the substrate material having the corundum structure include α-Al2O3 (sapphire substrate) or α-Ga2O3, and more suitable examples include a-plane sapphire substrate, m-plane sapphire substrate, r-plane sapphire substrate, c-plane sapphire substrate, and α-type gallium oxide substrate (a-plane, m-plane, or r-plane). Examples of the base substrate mainly made of a substrate material having a β-gallium structure include a β-Ga2O3 substrate, or a mixed crystal substrate containing Ga2O3 and Al2O3, with Al2O3 being more than 0 wt% and 60 wt% or less. Examples of the base substrate mainly made of a substrate material having a hexagonal structure include a SiC substrate, a ZnO substrate, and a GaN substrate.
[0027] In the present invention, an annealing treatment may be performed after the film formation step. The annealing temperature is not particularly limited as long as it does not impede the object of the present invention, and is usually 300°C to 650°C, and preferably 350°C to 550°C. The annealing time is usually 1 minute to 48 hours, preferably 10 minutes to 24 hours, and more preferably 30 minutes to 12 hours. The annealing may be performed in any atmosphere as long as it does not impede the object of the present invention, but is preferably an oxygen-free atmosphere, and more preferably a nitrogen atmosphere.
[0028] In the present invention, the semiconductor film may be provided directly on the substrate, or may be provided via another layer such as a buffer layer or a stress relaxation layer. The means for forming each layer is not particularly limited and may be a known means, but in the present invention, a mist CVD method is preferred.
[0029] In the present invention, the semiconductor film may be used as the semiconductor region in a semiconductor device after being peeled off from the base or the like by a known means, or may be used as it is as the semiconductor region in a semiconductor device.
[0030] The barrier height adjustment region is not particularly limited as long as it is a region in which the barrier height between the barrier electrode or the semiconductor region is greater than the barrier height at the interface between the semiconductor region and the barrier electrode. The barrier height adjustment region is usually mainly composed of a conductive material that makes the barrier height between the barrier electrode or the semiconductor region greater than the barrier height at the interface between the semiconductor region and the barrier electrode. Here, the term "main component" means that the conductive material is preferably contained in an atomic ratio of 50% or more, more preferably 70% or more, and even more preferably 90% or more of the total components of the barrier height adjustment region, and may be 100%. The conductive material is not particularly limited as long as it does not impede the object of the present invention, but is preferably a metal oxide or a metal. Examples of the metal oxide include those exemplified as the main component of the semiconductor region. Examples of the metal include those exemplified as the barrier electrode. The barrier height may be adjusted by using a known means to control the oxygen concentration, impurity concentration, interface state density, termination structure, crystal structure, or surface unevenness, or to modulate the work function or electron affinity. In the present invention, the barrier height adjusting region is preferably mainly composed of a p-type semiconductor. Examples of the p-type semiconductor include crystalline oxide semiconductors that are p-type doped with a p-type dopant (preferably Mg, Zn, or Ca). The p-type semiconductor preferably has a corundum structure or a hexagonal structure, and more preferably has a corundum structure. In the present invention, the p-type semiconductor is preferably an oxide semiconductor containing gallium, more preferably an InAlGaO-based semiconductor, and most preferably contains α-Ga2O3 or a mixed crystal thereof as a main component. The p-type semiconductor preferably used in the barrier height adjusting layer can be obtained by, for example, adding a p-type dopant and hydrobromic acid to a raw material solution containing a metal, and performing a mist CVD method. The steps, means, and conditions of the mist CVD method may be the same as the atomization / dropletization step, transport step, and film formation step, as well as the means and conditions described above. In the present invention, it is preferable that the barrier height of the Schottky barrier between the barrier height adjustment layer and the barrier electrode is adjusted to 1 eV or more. By adjusting the barrier height to such a preferable value, the semiconductor characteristics (e.g., switching characteristics, etc.) of the semiconductor device of the present invention can be further improved. The number of the barrier height adjustment regions is not particularly limited as long as it is 2 or more. In the present invention, it is preferable that the number of the barrier height adjustment regions is 3 or more, since the adjustment of the barrier height can be performed more effectively and the semiconductor characteristics of the semiconductor device can be improved, and it is more preferable that the number is 4 or more.
[0031] The means for forming the barrier height adjusting region is not particularly limited as long as it does not impede the object of the present invention, and may be a known means. For example, a means for forming a plurality of trenches in the surface of the interface side between the semiconductor region and the barrier electrode, and then forming a film consisting of the main component of the barrier height adjusting region in the trenches can be mentioned. In addition, for example, a means for modifying a part of the semiconductor region using a known surface treatment means such as dry etching, wet etching, plasma treatment, ultraviolet treatment, heat treatment, or surface treatment with an organic solvent or organic acid, and then forming a barrier electrode in the surface modified region to adjust the barrier height to form a barrier height adjusting region, or a means for forming a barrier height adjusting region by performing a heat treatment (e.g., electron beam annealing, laser annealing, etc.) or ultraviolet treatment on a part of the interface where the semiconductor region and the barrier electrode form a junction after or during the interface formation. Furthermore, in the present invention, the barrier height adjusting region may be formed by combining the above means. The means for forming the barrier height adjusting region may be carried out in a vacuum atmosphere, an air atmosphere, or a specific gas atmosphere.
[0032] Moreover, the semiconductor device of the present invention usually includes an ohmic electrode. The ohmic electrode may be made of a known electrode material, and is not particularly limited as long as it does not impede the object of the present invention, but preferably contains a metal of group 4 or group 11 of the periodic table. The metal of group 4 or group 11 of the periodic table suitable for use in the ohmic electrode may be the same as the metal contained in the Schottky electrode. The ohmic electrode may be a single metal layer or may contain two or more metal layers. The means for forming the ohmic electrode is not particularly limited, and examples of such means include known means such as vacuum deposition and sputtering. The metal constituting the ohmic electrode may be an alloy. In the present invention, the ohmic electrode preferably contains Ti and / or Au.
[0033] Preferred embodiments of the present invention will now be described in more detail with reference to the drawings, but the present invention is not limited to these embodiments.
[0034] FIG. 1 shows a junction barrier Schottky diode (JBS) according to a preferred embodiment of the present invention. The semiconductor device of FIG. 1 includes a semiconductor region 3, a barrier electrode 2 provided on the semiconductor region and capable of forming a Schottky barrier between the semiconductor region and the barrier electrode 2, and a barrier height adjustment layer provided between the barrier electrode 2 and the semiconductor region 3 and capable of forming a Schottky barrier with a barrier height greater than the barrier height of the Schottky barrier of the barrier electrode 2 between the semiconductor region 3. The barrier height adjustment layer 1 is embedded in the semiconductor region 3. In the present invention, it is preferable that the barrier height adjustment layers are provided at regular intervals, and it is more preferable that the barrier height adjustment regions are provided between both ends of the barrier electrode and the semiconductor region. With this preferred embodiment, the JBS is configured to have better thermal stability and adhesion, a greater reduction in leakage current, and better semiconductor properties such as breakdown voltage. The semiconductor device of FIG. 1 includes an ohmic electrode 4 on the semiconductor region 3.
[0035] 1 may be formed by any known means without any particular limitation as long as it does not impede the object of the present invention, for example, by forming a film by a vacuum deposition method, a CVD method, a sputtering method, various coating techniques, etc., followed by patterning by a photolithography method, or by directly patterning by a printing technique, etc.
[0036] A preferred manufacturing process of the semiconductor device of FIG. 1 will be described below with reference to FIG. 2. FIG. 2(a) shows a laminate in which an ohmic electrode 4 is laminated on a semiconductor substrate as a semiconductor region 3, and a plurality of trenches are formed on the opposite surface. Then, a barrier height adjustment layer 1 is formed in the trench of the semiconductor region 3 by photolithography on the laminate of FIG. 2(a), as shown in FIG. 2(b). After obtaining the laminate of FIG. 2(b), a barrier electrode 2 is formed on the barrier height adjustment layer 1 and the semiconductor region 3 by the dry method (preferably vacuum deposition or sputtering) or the wet method, etc., to obtain the laminate of FIG. 2(c). The laminate of FIG. 2(c) has a structure in which the barrier height adjustment layer 1 is embedded in the semiconductor region 3, and therefore has particularly excellent pressure resistance.
[0037] FIG. 3 shows a junction barrier Schottky diode (JBS) according to a preferred embodiment of the present invention. The semiconductor device in FIG. 3 differs from the semiconductor device in FIG. 1 in that a guard ring 5 is provided around the outer periphery of the barrier electrode. This configuration makes it possible to obtain a semiconductor device with better semiconductor characteristics such as breakdown voltage. In the present invention, the breakdown voltage can be improved more effectively by embedding a part of the guard ring 5 in the surface of the semiconductor region 3. Furthermore, by using a metal with a high barrier height for the guard ring, the guard ring can be provided industrially advantageously together with the formation of the barrier electrode, and can be formed without significantly affecting the semiconductor region or deteriorating the on-resistance.
[0038] The guard ring is usually made of a material with a high barrier height. Examples of the material used for the guard ring include conductive materials with a barrier height of 1 eV or more, and may be the same as the electrode material. In the present invention, the material used for the guard ring is preferably the metal, since it has a high degree of freedom in designing the pressure-resistant structure, can provide many guard rings, and can flexibly improve the pressure resistance. The shape of the guard ring is not particularly limited, and examples include a square shape, a circular shape, a U-shape, an L-shape, and a strip shape. In the present invention, a square shape or a circular shape is preferable. The number of guard rings is not particularly limited, but is preferably 3 or more, more preferably 6 or more.
[0039] Hereinafter, a preferred manufacturing process of the semiconductor device of FIG. 3 will be described with reference to FIG. 4 and FIG. 5. FIG. 4(a) shows a laminate in which an ohmic electrode 4 is laminated on a semiconductor substrate as a semiconductor region 3, and a plurality of trenches are formed on the opposite surface. Then, for the laminate of FIG. 4(a), a barrier height adjusting region 1 is formed on the semiconductor region 3 by photolithography as shown in FIG. 4(b), and then the surface of the semiconductor region 3 is exposed as shown in FIG. 4(c). In the laminates of FIG. 4(b) and (c), a barrier height adjusting region 1, a semiconductor region 3, and an ohmic electrode 4 are laminated. After obtaining the laminate of FIG. 4(c), a barrier electrode 2 is formed on the barrier height adjusting layer 1 and the semiconductor region 3 by the dry method (preferably vacuum deposition method or sputtering) or the wet method, etc., to obtain a laminate of FIG. 4(d).
[0040] Then, the laminate of FIG. 4(d) is etched using a photolithography method to remove a part of the barrier electrode 2 and a part of the semiconductor region 3 as shown in FIG. 5(e). After obtaining the laminate of FIG. 5(e), a guard ring 5 is formed on the semiconductor region 3 exposed on the surface by the dry method (preferably vacuum deposition or sputtering) or the wet method, etc., to obtain the laminate of FIG. 5(f). The laminate of FIG. 5(f) includes a guard ring 5, a barrier electrode 2, a barrier height adjustment layer 1, a semiconductor region 3, and an ohmic electrode 4, which are laminated. After obtaining the laminate of FIG. 5(f), etching is performed using a photolithography method to remove unnecessary parts, to obtain the laminate of FIG. 5(g). The laminate of FIG. 5(g) has a barrier height adjustment layer 1 embedded in the semiconductor region 3 and a guard ring 5 with an embedded structure in the periphery of the semiconductor region 3, and is therefore superior in terms of withstand voltage, etc. In the above description, the guard ring 5 is formed last, but in the present invention, it is also preferable to form the guard ring 5 before forming the barrier electrode 2. By forming the guard ring in this manner, the influence of the metal during the electrode formation can be suppressed.
[0041] FIG. 11 shows a junction barrier Schottky diode (JBS) according to a preferred embodiment of the present invention. The semiconductor device of FIG. 11 includes a semiconductor region 3, a barrier electrode 2 provided on the semiconductor region and capable of forming a Schottky barrier between the semiconductor region and the barrier electrode 2, and a barrier height adjustment layer provided between the barrier electrode 2 and the semiconductor region 3 and capable of forming a Schottky barrier with a barrier height greater than the barrier height of the Schottky barrier of the barrier electrode 2 between the semiconductor region 3. The barrier height adjustment layer 1 is embedded in the semiconductor region 3 and protrudes from the semiconductor region 3 into the barrier electrode 2. In the present invention, it is preferable that the barrier height adjustment layers are provided at regular intervals, and it is more preferable that the barrier height adjustment regions are provided between both ends of the barrier electrode and the semiconductor region. This preferred embodiment allows the JBS to have better thermal stability and adhesion, a better reduction in leakage current, a better suppression of electric field concentration, and better semiconductor properties such as a lower contact resistance. The semiconductor device of FIG. 11 includes an ohmic electrode 4 on the semiconductor region 3 on the opposite side to the barrier electrode 2.
[0042] The means for forming each layer of the semiconductor device in FIG. 11 may be the means for forming each layer described above.
[0043] Hereinafter, a preferred manufacturing process of the semiconductor device of FIG. 11 will be described with reference to FIG. 12. FIG. 12(a) shows a semiconductor substrate as a semiconductor region 3 having a plurality of trenches formed on the surface. Then, a p-type oxide semiconductor containing gallium is formed as a barrier height adjustment layer 1 on the semiconductor substrate of FIG. 12(a) by mist CVD to obtain a laminate shown in FIG. 12(b). The obtained laminate is etched using a photolithography method to remove unnecessary portions to obtain a laminate shown in FIG. 12(c). After obtaining the laminate of FIG. 2(c), a barrier electrode 2 is formed on the barrier height adjustment layer 1 and the semiconductor region 3 by the dry method (preferably vacuum deposition method or sputtering) or the wet method to obtain a laminate of FIG. 12(d). The laminate of FIG. 12(d) has a structure in which the barrier height adjustment layer 1 is embedded in the semiconductor region 3 and protrudes into the barrier electrode 2, so that it is possible to suppress electric field concentration and reduce contact resistance, and is particularly useful for a semiconductor device having excellent voltage resistance.
[0044] FIG. 13 shows a junction barrier Schottky diode (JBS) according to a preferred embodiment of the present invention. The semiconductor device of FIG. 13 includes a semiconductor region 3, a barrier electrode 2 that is provided on the semiconductor region and capable of forming a Schottky barrier between the semiconductor region and the barrier electrode 2, and a barrier height adjustment layer that is provided between the barrier electrode 2 and the semiconductor region 3 and capable of forming a Schottky barrier with a barrier height greater than the barrier height of the Schottky barrier of the barrier electrode 2 between the semiconductor region 3. The barrier height adjustment layer 1 is laminated on the semiconductor region 3 and protrudes into the barrier electrode 2. In the present invention, it is preferable that the barrier height adjustment layers are provided at regular intervals, and it is more preferable that the barrier height adjustment regions are provided between both ends of the barrier electrode and the semiconductor region. This preferred embodiment allows the JBS to have better thermal stability and adhesion, a greater reduction in leakage current, a greater suppression of electric field concentration, and better semiconductor properties such as a lower contact resistance. The semiconductor device of FIG. 13 includes an ohmic electrode 4 on the semiconductor region 3 on the side opposite to the barrier electrode 2.
[0045] The means for forming each layer of the semiconductor device in FIG. 13 may be the means for forming each layer described above.
[0046] Hereinafter, a preferred manufacturing process of the semiconductor device of FIG. 13 will be described with reference to FIG. 14. FIG. 12(a) shows a semiconductor substrate as the semiconductor region 3. Then, a p-type oxide semiconductor containing gallium is formed as the barrier height adjustment layer 1 on the semiconductor substrate of FIG. 14(a) by mist CVD to obtain a laminate shown in FIG. 14(b). The obtained laminate is etched using a photolithography method to remove unnecessary parts, and a laminate shown in FIG. 14(c) is obtained. After obtaining the laminate of FIG. 14(c), a barrier electrode 2 is formed on the barrier height adjustment layer 1 and the semiconductor region 3 by the dry method (preferably vacuum deposition method or sputtering) or the wet method, etc., to obtain a laminate of FIG. 14(d). The laminate of FIG. 14(d) has a structure in which the barrier height adjustment layer 1 is embedded in the semiconductor region 3 and protrudes into the barrier electrode 2, so that electric field concentration can be suppressed and contact resistance can be reduced, and it is particularly useful for a semiconductor device with excellent voltage resistance.
[0047] FIG. 15 shows a junction barrier Schottky diode (JBS) which is one of the preferred embodiments of the present invention. The semiconductor device in FIG. 15 differs from the semiconductor device in FIG. 11 in that a guard ring 5 is provided on the outer periphery of the barrier electrode. This configuration makes it possible to obtain a semiconductor device with better semiconductor characteristics such as breakdown voltage. In the present invention, as shown in FIG. 17, a part of the guard ring 5 is embedded in the surface of the semiconductor region 3, so that the breakdown voltage can be improved more effectively. Furthermore, by using a metal with a high barrier height for the guard ring, the guard ring can be provided industrially advantageously together with the formation of the barrier electrode, and can be formed without affecting the semiconductor region much and without deteriorating the on-resistance.
[0048] FIG. 16 shows a junction barrier Schottky diode (JBS) which is one of the preferred embodiments of the present invention. The semiconductor device in FIG. 16 differs from the semiconductor device in FIG. 13 in that a guard ring 5 is provided on the outer periphery of the barrier electrode. This configuration makes it possible to obtain a semiconductor device with better semiconductor characteristics such as breakdown voltage. In the present invention, as shown in FIG. 18, a part of the guard ring 5 is embedded in the surface of the semiconductor region 3, so that the breakdown voltage can be improved more effectively. Furthermore, by using a metal with a high barrier height for the guard ring, the guard ring can be provided industrially advantageously together with the formation of the barrier electrode, and can be formed without affecting the semiconductor region much and without deteriorating the on-resistance.
[0049] The semiconductor device is particularly useful as a power device. Examples of the semiconductor device include diodes and transistors (e.g., MESFETs), among which diodes are preferred, and junction barrier Schottky diodes (JBSs) are more preferred.
[0050] In addition to the above, the semiconductor device of the present invention can be suitably used as a power module, inverter or converter by using known means, and can also be suitably used in a semiconductor system using a power supply device. The power supply device can be manufactured from the semiconductor device or as the semiconductor device by connecting to a wiring pattern or the like by using known means. FIG. 6 shows an example of a power supply system. FIG. 6 shows a power supply system using a plurality of the power supplies and a control circuit. The power supply system can be used in a system device in combination with an electronic circuit as shown in FIG. 7. FIG. 8 shows an example of a power supply circuit diagram of a power supply device. FIG. 8 shows a power supply circuit of a power supply device consisting of a power circuit and a control circuit, in which a DC voltage is switched at high frequency by an inverter (composed of MOSFETs: A to D) and converted to AC, then insulated and transformed by a transformer, rectified by a rectifier MOSFET (A to B'), smoothed by a DCL (smoothing coils L1, L2) and a capacitor, and a DC voltage is output. At this time, a voltage comparator compares the output voltage with a reference voltage, and a PWM control circuit controls the inverter and rectifier MOSFET so as to obtain a desired output voltage. EXAMPLES
[0051] (Reference Example 1: Adjustment of Barrier Height by Annealing) 1-1. Formation of n-type semiconductor layer 1-1-1. Film deposition equipment The mist CVD apparatus 19 used in the reference example will be described with reference to Fig. 9. The mist CVD apparatus 19 includes a susceptor 21 on which a substrate 20 is placed, a carrier gas supply means 22a for supplying a carrier gas, a flow rate control valve 23a for adjusting the flow rate of the carrier gas sent from the carrier gas supply means 22a, a carrier gas (dilution) supply means 22b for supplying a carrier gas (dilution), a flow rate control valve 23b for adjusting the flow rate of the carrier gas sent from the carrier gas (dilution) supply means 22b, a mist generating source 24 in which a raw material solution 24a is stored, a container 25 in which water 25a is stored, an ultrasonic vibrator 26 attached to the bottom surface of the container 25, a supply pipe 27 made of a quartz tube with an inner diameter of 40 mm, and a heater 28 installed around the supply pipe 27. The susceptor 21 is made of quartz, and the surface on which the substrate 20 is placed is inclined from the horizontal plane. Both the supply pipe 27 and the susceptor 21 that constitute the film formation chamber are made of quartz, thereby preventing impurities originating from the apparatus from being mixed into the film formed on the substrate 20 .
[0052] 1-1-2. Preparation of raw material solution A 0.1 M aqueous gallium bromide solution containing 20% hydrobromic acid by volume was used as a raw material solution.
[0053] 1-1-3. Preparation for film formation The raw material solution 24a obtained in 1-1-2 above was accommodated in the mist generating source 24. Next, a sapphire substrate was placed on the susceptor 21 as the substrate 20, and the heater 28 was operated to raise the temperature in the film formation chamber 27 to 480°C. Next, the flow rate control valves 23a and 23b were opened to supply carrier gas from the carrier gas supply means 22a and 22b, which are the carrier gas sources, into the film formation chamber 27, and the atmosphere in the film formation chamber 27 was sufficiently replaced with the carrier gas, after which the flow rate of the carrier gas was adjusted to 5 L / min and the flow rate of the carrier gas (dilution) was adjusted to 0.5 L / min. Nitrogen was used as the carrier gas.
[0054] 1-1-4. Semiconductor film formation Next, the ultrasonic vibrator 26 was vibrated at 2.4 MHz, and the vibration was propagated to the raw material solution 24a through the water 25a, thereby atomizing the raw material solution 24a to generate mist. This mist was introduced into the film formation chamber 27 by the carrier gas, and reacted in the film formation chamber 27 at atmospheric pressure and 510°C to form a semiconductor film on the substrate 20. The film thickness was 2.5 μm, and the film formation time was 180 minutes.
[0055] 1-1-5.Evaluation When the phase of the film obtained in 1-1-4. above was identified using an XRD diffractometer, it was found to be α-Ga2O3.
[0056] 1-2. Formation of n+ type semiconductor layer A semiconductor film was formed on the n-type semiconductor layer obtained in 1-1 above in the same manner as in 1-1 above, except that a 0.05M aqueous solution of gallium acetylacetonate was used as the raw material solution, containing 1.5% hydrochloric acid and 0.2% tin chloride by volume. The phase of the obtained film was identified using an XRD diffractometer, and the obtained film was α-Ga2O3.
[0057] 1-3. Formation of Ohmic Electrodes A Ti layer and an Au layer were laminated on the n+ type semiconductor layer by electron beam deposition. The Ti layer had a thickness of 35 nm, and the Au layer had a thickness of 175 nm.
[0058] 1-4. Formation of Schottky electrode After removing the sapphire substrate, a Pt layer was laminated on the n-type semiconductor layer by electron beam deposition. The layer was then annealed at 400°C for 30 seconds in a nitrogen atmosphere using a rapid annealing apparatus (RTA) to form an annealed Pt layer. A non-annealed Pt layer was also formed by photolithography and etching.
[0059] 1-5.Evaluation An IV measurement was carried out. As a result, the barrier height of the unannealed Pt layer was 1.5 eV, and the barrier height of the annealed Pt layer was 0.9 eV. The IV measurement results of the annealed Pt layer are shown in Figure 10.
[0060] (Reference Example 2: Adjusting the barrier height using p-type semiconductors) In Reference Example 2, adjustment of the barrier height by a p-type semiconductor was evaluated. 2-1. Formation of p-type semiconductor layer A semiconductor film was formed in the same manner as in 1-1 above, except that a sapphire substrate having an n+ type semiconductor layer formed on the surface by mist CVD was used as the substrate, gallium bromide and magnesium bromide were mixed with ultrapure water as the raw material solution, and an aqueous solution was adjusted so that the atomic ratio of magnesium to gallium was 1:0.01 and gallium bromide was 0.1 mol / L, and a solution containing 20% hydrohalic acid by volume was used, the flow rate of the carrier gas was 1 L / min, the flow rate of the carrier gas (dilution) was 1 L / min, the film formation temperature was 520°C, and the film formation time was 60 minutes. The phase of the film was identified using an XRD diffractometer, and the film obtained using hydrobromic acid as hydrohalic acid was α-Ga2O3.
[0061] 2-2.Evaluation In order to confirm whether magnesium functions normally as a p-type dopant in the p-type semiconductor layer, IV measurements were performed on the α-Ga2O3 film obtained in 2-1 above. As a result, it showed excellent rectification, and the n+ type semiconductor layer and the p-type semiconductor layer formed a good PN junction. As is clear from the IV measurement results, since magnesium functions normally as a p-type dopant, it was found that the barrier height can be adjusted by forming a p-type semiconductor. [Industrial Applicability]
[0062] The semiconductor device of the present invention can be used in a wide variety of fields, including semiconductors (eg, compound semiconductor electronic devices), electronic components, electrical equipment components, optical and electrophotographic related devices, and industrial materials, but is particularly useful as a power device. [Explanation of symbols]
[0063] 1. Barrier height adjustment layer 2 Barrier Electrode 3. Semiconductors 4 Ohmic electrodes 5 Guard Ring 19 Mist CVD Equipment 20 Substrate 21 Susceptor 22a Carrier gas supply means 22b Carrier gas (dilution) supply means 23a Flow control valve 23b Flow control valve 24 Mist Source 24a Raw material solution 25 Container 25a water 26 Ultrasonic transducer 27 Supply pipe 28 Heater 29 Exhaust port
Claims
1. A semiconductor device comprising at least a semiconductor region and a barrier electrode provided on the semiconductor region, the semiconductor region containing a crystalline oxide semiconductor containing gallium as a main component, a barrier height adjusting region being provided between the semiconductor region and the barrier electrode, in which a barrier height between the barrier electrode or the semiconductor region is greater than a barrier height at an interface between the semiconductor region and the barrier electrode, the barrier height adjusting region being mainly composed of a p-type oxide semiconductor which is a metal oxide having a different composition from the crystalline oxide semiconductor and does not contain a p-type dopant, or being mainly composed of a metal oxide semiconductor having a different composition from the crystalline oxide semiconductor and not containing gallium oxide.
2. A semiconductor device comprising at least a semiconductor region and a barrier electrode provided on the semiconductor region, wherein the semiconductor region contains a crystalline oxide semiconductor containing gallium as a main component, and a barrier height adjustment region is provided between the semiconductor region and the barrier electrode, in which the barrier height between the semiconductor region and the barrier electrode is greater than the barrier height at the interface between the semiconductor region and the barrier electrode, the crystalline oxide semiconductor has a β gallium structure, and the barrier height adjustment region is mainly composed of a p-type oxide semiconductor having a composition different from that of the crystalline oxide semiconductor.
3. 3. The semiconductor device according to claim 1, wherein the barrier height adjusting region is a barrier height adjusting layer formed on the semiconductor region.
4. 4. The semiconductor device according to claim 1, wherein the barrier height adjusting region is mainly composed of a p-type oxide semiconductor containing a metal element other than gallium.
5. 5. The semiconductor device according to claim 1, wherein the barrier height adjusting region contains a p-type dopant.
6. A semiconductor device comprising at least a semiconductor region and a barrier electrode provided on the semiconductor region, the semiconductor region containing a crystalline oxide semiconductor containing gallium as a main component, a barrier height adjustment region being provided between the semiconductor region and the barrier electrode, in which a barrier height between the barrier electrode or the semiconductor region is greater than a barrier height at an interface between the semiconductor region and the barrier electrode, the barrier height adjustment region being mainly composed of a p-type oxide semiconductor and not containing a p-type dopant or not containing gallium oxide, and the barrier height adjustment region being a barrier height adjustment layer formed on the semiconductor region.
7. A semiconductor device comprising at least a semiconductor region and a barrier electrode provided on the semiconductor region, wherein the semiconductor region contains a crystalline oxide semiconductor containing gallium as a main component, and a barrier height adjustment region is provided between the semiconductor region and the barrier electrode, in which the barrier height with the barrier electrode or the semiconductor region is greater than the barrier height at the interface between the semiconductor region and the barrier electrode, the crystalline oxide semiconductor has a β gallium structure, and the barrier height adjustment region is mainly composed of a p-type oxide semiconductor and is a barrier height adjustment layer formed on the semiconductor region.
8. A semiconductor device comprising at least a semiconductor region and a barrier electrode provided on the semiconductor region, the semiconductor region containing a crystalline oxide semiconductor containing gallium as a main component, a barrier height adjusting region being provided between the semiconductor region and the barrier electrode, in which a barrier height between the semiconductor region and the barrier electrode or the barrier height adjusting region is greater than a barrier height at an interface between the semiconductor region and the barrier electrode, and the barrier height adjusting region is mainly composed of a p-type oxide semiconductor containing a metal element other than gallium.
9. The semiconductor device described in claim 8, wherein the barrier height adjustment region is mainly composed of a p-type oxide semiconductor which is a metal oxide and does not contain a p-type dopant, or does not contain gallium oxide.
10. A semiconductor device comprising at least a semiconductor region and a barrier electrode provided on the semiconductor region, wherein the semiconductor region contains a crystalline oxide semiconductor containing gallium as a main component, and a barrier height adjusting region is provided between the semiconductor region and the barrier electrode, in which a barrier height between the semiconductor region and the barrier electrode or the barrier height between the semiconductor region and the barrier electrode is greater than a barrier height at an interface between the semiconductor region and the barrier electrode, and the barrier height adjusting region is mainly composed of a p-type oxide semiconductor which is a metal oxide semiconductor not containing gallium oxide and contains a p-type dopant.
11. The semiconductor device according to claim 1, wherein the crystalline oxide semiconductor has a β-gallium structure.
12. A semiconductor device comprising at least a semiconductor region and a barrier electrode provided on the semiconductor region, wherein the semiconductor region contains a crystalline oxide semiconductor containing gallium as its main component, and a barrier height adjustment region is provided between the semiconductor region and the barrier electrode, in which the barrier height with the barrier electrode or the semiconductor region is greater than the barrier height at the interface between the semiconductor region and the barrier electrode, the crystalline oxide semiconductor has a β gallium structure, and the barrier height adjustment region is mainly composed of a p-type oxide semiconductor and contains a p-type dopant.
13. The semiconductor region is α-Ga 2 O 3 11. The semiconductor device according to claim 1, 6, or 8, which contains the mixed crystal thereof as a main component.
14. 14. The semiconductor device according to claim 1, wherein the barrier height adjusting region contains gallium.
15. 15. The semiconductor device according to claim 1, wherein a plurality of the barrier height adjusting regions are provided on the surface of the semiconductor region.
16. 16. The semiconductor device according to claim 1, wherein the barrier height adjusting regions are provided between both ends of the barrier electrode and the semiconductor region.
17. 17. The semiconductor device according to claim 1, wherein the barrier height adjusting region protrudes into the barrier electrode.
18. 18. The semiconductor device according to claim 1, wherein a guard ring is provided on the outer periphery of the barrier electrode.
19. 20. The semiconductor device according to claim 18, wherein a part or the whole of the guard ring is embedded in the surface of the semiconductor region.
20. 20. The semiconductor device according to claim 1, wherein a barrier height at an interface between the barrier electrode and the barrier height adjusting region is 1 eV or more.
21. 21. The semiconductor device according to claim 1, wherein the barrier electrode is made of a metal.
22. 22. The semiconductor device according to claim 1, wherein the semiconductor region contains a gallium compound as a main component.
23. 23. The semiconductor device according to claim 1, wherein the barrier height adjusting region contains, as a main component, a p-type oxide semiconductor having a corundum structure or a hexagonal structure.
24. The semiconductor device according to any one of claims 1 to 23, which is a diode.
25. 25. The semiconductor device according to claim 1, which is a junction barrier Schottky diode.
26. The semiconductor device according to any one of claims 1 to 25, which is a power device.
27. A semiconductor system comprising a semiconductor device, the semiconductor device being the semiconductor device according to any one of claims 1 to 26.
Citation Information
Patent Citations
Semiconductor element having schottoky barriercontact
JP1977101970A
Shottky barrier semiconductor device
JP1993326925A
Semiconductor device including heterojunction barrier region and method for manufacturing the same
JP2013522876A
Improved Schottky rectifier
JP2013545295A
Wide gap semiconductor device and method for manufacturing the same
JP2014078660A