Resin materials and multilayer printed wiring boards
A maleimide compound-based resin material with specific properties enhances embeddability, suppresses wetting, and reduces undulation in multilayer printed wiring boards, addressing issues of conventional resin materials.
Patent Information
- Application Number
- JP2020130790
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-08-01
- Filing Date
- 2020-07-31
- Publication Date
- 2024-12-09
- Estimated Expiration
- 2040-07-31
AI Technical Summary
Conventional resin materials used in multilayer printed wiring boards face issues with embeddability into uneven surfaces, excessive wetting and spreading, and undulation in the formed insulating layers, making it difficult to control the thickness and achieve uniformity.
A resin material containing a maleimide compound with specific properties, including a weight average molecular weight between 1000 and 50000, and a haze of 5% or more in a cyclohexanone solution, is used, along with a curing accelerator, to improve embeddability, suppress wetting, and reduce undulation.
The resin material effectively improves embeddability into uneven surfaces, suppresses excessive wetting and spreading, and reduces undulation, resulting in a more uniform and controlled insulating layer thickness.
Smart Images

Figure 0007596091000008 
Figure 0007596091000001 
Figure 0007596091000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin material containing a maleimide compound. The present invention also relates to a multilayer printed wiring board using the resin material. [Background technology]
[0002] Conventionally, various resin materials have been used to obtain electronic components such as semiconductor devices, laminates, and printed wiring boards. For example, in a multilayer printed wiring board, a resin material is used to form an insulating layer for insulating between internal layers, or to form an insulating layer located on a surface layer. Wiring, which is generally metal, is laminated on the surface of the insulating layer. In addition, a resin film obtained by filming the resin material may be used to form the insulating layer. The resin material and the resin film are used as insulating materials for multilayer printed wiring boards, including build-up films.
[0003] The following Patent Document 1 discloses a resin composition containing a compound having a maleimide group, a divalent group having at least two imide bonds, and a saturated or unsaturated divalent hydrocarbon group. Patent Document 1 also describes that a cured product of this resin composition can be used as an insulating layer for a multilayer printed wiring board or the like.
[0004] The following Patent Document 2 discloses a resin composition for electronic materials that contains a bismaleimide compound having two maleimide groups and one or more polyimide groups having a specific structure. In the bismaleimide compound, the two maleimide groups are each independently bonded to both ends of the polyimide group via at least a first linking group in which eight or more atoms are linearly linked. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] WO2016 / 114286A1 [Patent Document 2] JP 2018-90728 A Summary of the Invention [Problem to be solved by the invention]
[0006] When forming an insulating layer using conventional resin materials such as those described in Patent Documents 1 and 2, the resin material may not be able to embed sufficiently into uneven surfaces on a substrate, the resin material may spread excessively, or undulations may occur in the formed insulating layer, making it difficult to control the thickness of the insulating layer.
[0007] The object of the present invention is to provide a resin material that can 1) enhance embedding properties into uneven surfaces, 2) suppress wet spreading, and 3) reduce undulations. Another object of the present invention is to provide a multilayer printed wiring board using the resin material. [Means for solving the problem]
[0008] According to a broad aspect of the present invention, there is provided a resin material comprising a maleimide compound and a curing accelerator, wherein when a maleimide compound-containing liquid containing 5% by weight of the maleimide compound and 95% by weight of cyclohexanone is obtained, the maleimide compound exhibits a property such that the haze of the maleimide compound-containing liquid is 5% or more, and the content of the maleimide compound is 5% by weight or more in 100% by weight of components in the resin material excluding inorganic fillers and solvents.
[0009] In a specific aspect of the resin material according to the present invention, the maleimide compound has a weight average molecular weight of 1,000 or more and 50,000 or less.
[0010] In a specific aspect of the resin material according to the present invention, the maleimide compound has a structure represented by the following formula (X):
[0011] [ka]
[0012] In the formula (X), R1 represents a tetravalent organic group.
[0013] In a specific aspect of the resin material according to the present invention, the maleimide compound has a skeleton derived from an aliphatic diamine compound.
[0014] In a specific aspect of the resin material according to the present invention, the aliphatic diamine compound has a ring structure including a cyclohexane skeleton.
[0015] In a specific aspect of the resin material according to the present invention, the resin material includes a thermoplastic resin, and the thermoplastic resin has a weight average molecular weight of 20,000 or more.
[0016] In a specific aspect of the resin material according to the present invention, the curing accelerator includes a photocuring accelerator.
[0017] In a specific aspect of the resin material according to the present invention, the resin material includes a curable compound, and the curable compound includes a curable compound having a weight average molecular weight of less than 1,500.
[0018] In a specific aspect of the resin material according to the present invention, the resin material includes a thermosetting compound and a curing agent, and the thermosetting compound includes an epoxy compound.
[0019] In a specific aspect of the resin material according to the present invention, the curing agent includes an active ester compound.
[0020] In a specific aspect of the resin material according to the present invention, the resin material contains an inorganic filler.
[0021] In a specific aspect of the resin material according to the present invention, the content of the inorganic filler is 50% by weight or more based on 100% by weight of the components excluding the solvent in the resin material.
[0022] In a specific aspect of the resin material according to the present invention, the inorganic filler is silica.
[0023] In a specific aspect of the resin material according to the present invention, the resin material is a resin film.
[0024] The resin material according to the present invention is suitably used for forming an insulating layer in a multilayer printed wiring board.
[0025] According to a broad aspect of the present invention, there is provided a multilayer printed wiring board comprising a circuit board, a plurality of insulating layers disposed on a surface of the circuit board, and a metal layer disposed between the plurality of insulating layers, wherein at least one of the plurality of insulating layers is a cured product of the resin material described above. Effect of the Invention
[0026] The resin material according to the present invention includes a maleimide compound and a curing accelerator. In the resin material according to the present invention, when a maleimide compound-containing liquid containing 5% by weight of the maleimide compound and 95% by weight of cyclohexanone is obtained, the maleimide compound exhibits a property that the cloudiness of the maleimide compound-containing liquid is 5% or more. In the resin material according to the present invention, the content of the maleimide compound is 5% by weight or more in 100% by weight of the components in the resin material excluding the inorganic filler and the solvent. Since the resin material according to the present invention has the above-mentioned configuration, 1) embedding ability into uneven surfaces can be improved, 2) wetting spread can be suppressed, and 3) undulation can be reduced. [Brief description of the drawings]
[0027] [Figure 1] FIG. 1 is a cross-sectional view showing a schematic diagram of a multilayer printed wiring board using a resin material according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0028] The present invention will be described in detail below.
[0029] The resin material according to the present invention contains a maleimide compound (hereinafter, may be referred to as "maleimide compound X") and a curing accelerator.
[0030] In the resin material according to the present invention, when a maleimide compound-containing liquid containing 5% by weight of the maleimide compound X and 95% by weight of cyclohexanone is obtained, the maleimide compound X is a maleimide compound that exhibits a property such that the haze of the maleimide compound-containing liquid is 5% or more.
[0031] In the resin material according to the present invention, the content of the maleimide compound X is 5% by weight or more based on 100% by weight of the components in the resin material excluding the inorganic filler and the solvent.
[0032] Since the resin material according to the present invention has the above-mentioned configuration, it is possible to achieve all of the following effects 1)-3): 1) the embedding ability into uneven surfaces can be improved, 2) the wetting spreading can be suppressed, and 3) undulation can be reduced.
[0033] Furthermore, when the resin material according to the present invention is a resin film such as a B-stage film, the flexibility of the resin film can be increased.
[0034] The present inventors have found that the use of the maleimide compound X in a resin material can achieve all of the above-mentioned effects 1)-3). The maleimide compound X is, for example, a maleimide compound capable of forming aggregates capable of scattering visible light. In conventional resin materials containing a maleimide compound, the cohesiveness of the maleimide compound is insufficient, and the viscosity of the resin material (varnish) is likely to increase or decrease, particularly depending on the molecular weight of the maleimide compound. For this reason, particularly when the molecular weight of the maleimide compound is large, the embeddability of the resin material in the uneven surface decreases, and particularly when the molecular weight of the maleimide compound is small, the wetting spread cannot be sufficiently suppressed, or the undulation may become large. In contrast, in the present invention, since the maleimide compound X exhibiting a certain degree of cohesiveness is used, it is possible to prevent the viscosity of the varnish from becoming excessively large, and the viscosity of the resin material can be improved. As a result, in the resin material according to the present invention, 1) the embeddability of the resin material in the uneven surface can be increased, 2) the wetting spread can be suppressed, and 3) the undulation can be reduced. In the resin material according to the present invention, even if the molecular weight of the maleimide compound X is large, all of the above-mentioned effects 1) to 3) can be achieved.
[0035] In addition, in the present invention, since the maleimide compound X exhibiting a certain degree of aggregability is used, even if the reaction equivalent is small, the functional groups can be made to exist relatively close to each other. Therefore, the reaction temperature can be lowered, and the resin material can be sufficiently cured. In addition, since the maleimide compound X has already aggregated, the shrinkage of the resin material during curing can be reduced in some cases. In particular, when the resin material is used after photocuring, the reaction temperature is lower than when it is used after thermal curing, and therefore the molecular mobility is low. In the present invention, since the functional groups can be made to exist relatively close to each other, the reaction efficiency can be increased even when it is used after photocuring. In addition, in the present invention, the surface roughness of the cured resin material can be suppressed from becoming excessively large when a roughening treatment is performed after precuring, particularly in the SAP process.
[0036] The resin material according to the present invention may be a resin composition or a resin film. The resin composition has fluidity. The resin composition may be in a paste form. The paste form includes a liquid form. In view of excellent handling properties, the resin material according to the present invention is preferably a resin film.
[0037] The resin material according to the present invention may be used after being thermally cured, photocured, or both thermally and photocured. The resin material according to the present invention is preferably a thermosetting resin material or a photocurable resin material, and more preferably a thermosetting resin material. When the resin material is a resin film, the resin film is preferably a thermosetting resin film or a photocurable resin film, and more preferably a thermosetting resin film.
[0038] Hereinafter, details of each component used in the resin material according to the present invention and applications of the resin material according to the present invention will be described.
[0039] [Maleimide compound X] The resin material according to the present invention contains the maleimide compound X. The maleimide compound X is preferably a thermosetting compound. The maleimide compound X may be used alone or in combination of two or more kinds.
[0040] The maleimide compound X is a maleimide compound that exhibits a property that, when a maleimide compound-containing liquid (hereinafter sometimes referred to as a "first maleimide compound-containing liquid") containing 5% by weight of the maleimide compound X and 95% by weight of cyclohexanone is obtained, the haze of the maleimide compound-containing liquid (first maleimide compound-containing liquid) is 5% or more.
[0041] The haze of the first maleimide compound-containing liquid is preferably 7% or more, more preferably 8% or more. When the haze of the first maleimide compound-containing liquid is equal to or more than the lower limit, the effect of the present invention can be more effectively exhibited. The upper limit of the haze of the first maleimide compound-containing liquid is not particularly limited. The haze of the first maleimide compound-containing liquid may be 20% or less, 15% or less, or 10% or less.
[0042] In addition, when a first maleimide compound-containing liquid cannot be prepared because the maleimide compound is not dissolved in cyclohexanone, for example, the maleimide compound does not correspond to the maleimide compound X of the present invention. In addition, when the first maleimide compound-containing liquid (5 wt % maleimide compound) is allowed to stand at 25° C. for 24 hours and the color of the first maleimide compound-containing liquid after standing varies from shade to shade, that is, when precipitation of the maleimide compound occurs, the maleimide compound does not correspond to the maleimide compound X of the present invention.
[0043] When a maleimide compound-containing liquid containing 10% by weight of the maleimide compound X and 90% by weight of cyclohexanone (hereinafter sometimes referred to as "second maleimide compound-containing liquid") is obtained, the haze of the maleimide compound-containing liquid (second maleimide compound-containing liquid) is preferably 8% or more, more preferably 10% or more, and even more preferably 15% or more. When the haze of the second maleimide compound-containing liquid is equal to or more than the lower limit, the effect of the present invention can be more effectively exhibited. The upper limit of the haze of the second maleimide compound-containing liquid is not particularly limited. The haze of the second maleimide compound-containing liquid may be 35% or less, 25% or less, or 20% or less.
[0044] The second maleimide compound-containing liquid is allowed to stand at 25° C. for 24 hours, and it is preferable that the color of the second maleimide compound-containing liquid after standing does not change shade.
[0045] The haze of the first and second maleimide compound-containing liquids can be measured using a haze meter (for example, "HM-150" manufactured by Murakami Color Research Laboratory).
[0046] The first maleimide compound-containing liquid and the second maleimide compound-containing liquid are prepared to determine whether the maleimide compound X has a specific property. In the resin material according to the present invention, the maleimide compound X does not have to be added as a first maleimide compound-containing liquid containing 5% by weight of the maleimide compound X and 95% by weight of cyclohexanone, and does not have to be added as a second maleimide compound-containing liquid containing 10% by weight of the maleimide compound X and 90% by weight of cyclohexanone. The concentration of the maleimide compound X added and the solvent for dissolving the maleimide compound X when preparing the resin material may be different from those described above.
[0047] In order to easily make the haze of the first and second maleimide compound-containing liquids satisfy the above range, the maleimide compound X preferably has a skeleton derived from pyromellitic dianhydride, and more preferably has a skeleton derived from an aliphatic diamine compound. In order to more easily make the haze of the first and second maleimide compound-containing liquids satisfy the above range, the maleimide compound X preferably has a skeleton derived from a reaction product of pyromellitic dianhydride and a diamine compound, and more preferably has a skeleton derived from a reaction product of pyromellitic dianhydride and an aliphatic diamine compound.
[0048] Even if the maleimide compound has a skeleton derived from pyromellitic dianhydride, the haze of the first and second maleimide compound-containing liquids may not satisfy the above range. Even if the maleimide compound has a skeleton derived from an aliphatic diamine compound, the haze of the first and second maleimide compound-containing liquids may not satisfy the above range. On the other hand, even if the maleimide compound does not have a skeleton derived from pyromellitic dianhydride, the haze of the first and second maleimide compound-containing liquids may satisfy the above range. Even if the maleimide compound does not have a skeleton derived from an aliphatic diamine compound, the haze of the first and second maleimide compound-containing liquids may satisfy the above range.
[0049] Examples of the diamine compound include dimer diamine, tricyclodecane diamine, 1,3-bis(aminomethyl)cyclohexane, 1,4-bis(aminomethyl)cyclohexane, bis(aminomethyl)norbornane, 3(4),8(9)-bis(aminomethyl)tricyclo[5.2.1.02,6]decane, 1,3-cyclohexanediamine, 1,4-cyclohexanediamine, isophoronediamine, 4,4'-methylenebis(cyclohexylamine), 4,4'-methylenebis(2-methylcyclohexylamine), 1,1-bis(4-aminomethyl)diamine, 1,2-diaminoethyldiamine, 1,3-diaminoethyldiamine, 1,4-diaminoethyl ... Examples of the diamine compounds include cyclohexane, 2,7-diaminofluorene, 4,4'-ethylenedianiline, 4,4'-methylenebis(2,6-diethylaniline), 4,4'-methylenebis(2-ethyl-6-methylaniline), 1,4-diaminobutane, 1,10-diaminodecane, 1,12-diaminododecane, 1,7-diaminoheptane, 1,6-diaminohexane, 1,5-diaminopentane, 1,8-diaminooctane, 1,3-diaminopropane, 1,11-diaminoundecane, and 2-methyl-1,5-diaminopentane. The diamine compounds may be used alone or in combination of two or more.
[0050] From the viewpoint of exerting the effects of the present invention more effectively, the diamine compound is preferably an aliphatic diamine compound, and is preferably a diamine compound having a dicyclopentadiene skeleton. From the viewpoint of exerting the effects of the present invention even more effectively, the aliphatic diamine compound preferably has a cyclohexyl ring, more preferably has a ring structure containing a cyclohexane skeleton, and even more preferably has a dicyclopentadiene skeleton. Examples of the ring structure containing a cyclohexane skeleton include a tricyclodecane ring, a norbornane ring, and an adamantane skeleton.
[0051] Examples of the dimer diamine include VERSAMINE 551 (trade name, manufactured by BASF Japan, 3,4-bis(1-aminoheptyl)-6-hexyl-5-(1-octenyl)cyclohexene), VERSAMINE 552 (trade name, manufactured by Cognics Japan, hydrogenated VERSAMINE 551), and PRIAMINE 1075 and PRIAMINE 1074 (trade names, all manufactured by Croda Japan).
[0052] It is preferable that the maleimide compound X does not have a skeleton derived from dimer diamine, or has a skeleton derived from dimer diamine and the average ratio of the skeleton derived from dimer diamine to the total structural units (100 mol %) of the skeleton derived from diamine compound is 50 mol % or less. In this case, the coefficient of linear thermal expansion of the cured product can be further reduced. In addition, the haze of the first and second maleimide compound-containing liquids can be easily adjusted to satisfy the above range.
[0053] Even if the maleimide compound does not have a skeleton derived from dimer diamine, the haze of the first and second maleimide compound-containing liquids may not satisfy the above range. Also, even if the maleimide compound has a skeleton derived from dimer diamine and the average proportion of skeletons derived from dimer diamine in 100 mol % of all structural units derived from diamine compounds is 50 mol % or less, the haze of the first and second maleimide compound-containing liquids may not satisfy the above range.
[0054] The maleimide compound X may have a skeleton derived from a reaction product of a diamine compound and an acid dianhydride other than pyromellitic dianhydride.
[0055] Examples of the acid dianhydride other than pyromellitic dianhydride include tetracarboxylic dianhydrides. Examples of the tetracarboxylic dianhydride include 3,3',4,4'-benzophenone tetracarboxylic dianhydride, 3,3',4,4'-biphenylsulfone tetracarboxylic dianhydride, 1,4,5,8-naphthalene tetracarboxylic dianhydride, 2,3,6,7-naphthalene tetracarboxylic dianhydride, 3,3',4,4'-biphenyl ether tetracarboxylic dianhydride, 3,3',4,4'-dimethyldiphenylsilane tetracarboxylic dianhydride, 3,3',4,4'-tetraphenylsilane tetracarboxylic dianhydride, 1,2,3,4-furan tetracarboxylic dianhydride, 4,4'-bis(3,4-dicarboxyphenoxy)diphenyl sulfide dianhydride, and the like. Examples of the dianhydride include water, 4,4'-bis(3,4-dicarboxyphenoxy)diphenylsulfone dianhydride, 4,4'-bis(3,4-dicarboxyphenoxy)diphenylpropane dianhydride, 3,3',4,4'-perfluoroisopropylidenediphthalic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, bis(phthalic acid)phenylphosphine oxide dianhydride, p-phenylene-bis(triphenylphthalic acid) dianhydride, m-phenylene-bis(triphenylphthalic acid) dianhydride, bis(triphenylphthalic acid)-4,4'-diphenyl ether dianhydride, and bis(triphenylphthalic acid)-4,4'-diphenylmethane dianhydride.
[0056] From the viewpoint of lowering the dielectric tangent of the cured product and enhancing the thermal dimensional stability of the cured product, the number of maleimide skeletons in the maleimide compound X is preferably 2 or more, more preferably 3 or more, and preferably 10 or less, more preferably 5 or less.
[0057] From the viewpoint of further lowering the dielectric tangent of the cured product and further increasing the thermal dimensional stability of the cured product, it is preferable that the maleimide compound X has a maleimide skeleton at both ends.
[0058] The maleimide compound X may or may not have a branched structure.
[0059] In order to more effectively exert the effects of the present invention, the maleimide compound X preferably has a structure represented by the following formula (X).
[0060] [ka]
[0061] In the above formula (X), R1 represents a tetravalent organic group.
[0062] The maleimide compound X can be prepared, for example, as follows: A diamine compound, a dimer diamine compound, and pyromellitic dianhydride are reacted to obtain a first reactant, and the obtained first reactant is reacted with maleic anhydride.
[0063] The weight average molecular weight of the maleimide compound X is preferably 1000 or more, more preferably 3000 or more, even more preferably more than 3100, even more preferably more than 4500, even more preferably more than 5000, particularly preferably 7500 or more, and most preferably 8000 or more. The weight average molecular weight of the maleimide compound X is preferably 50000 or less, more preferably 30000 or less, even more preferably 20000 or less, particularly preferably 18000 or less, and most preferably 15000 or less. When the weight average molecular weight is equal to or more than the lower limit, the linear expansion coefficient can be kept low, and the viscosity of the resin material can be made moderate. When the weight average molecular weight is greater than 50000, the melt viscosity of the resin material becomes higher than when the weight average molecular weight is equal to or less than 50000, and the embedding property for the uneven surface may decrease. When the weight average molecular weight is equal to or more than the lower limit and equal to or less than the upper limit, the aggregated site is efficiently etched, and the desmear property can be improved.
[0064] The weight average molecular weight is a weight average molecular weight measured by gel permeation chromatography (GPC) and calculated as polystyrene.
[0065] From the viewpoint of further increasing the thermal dimensional stability of the cured product and further increasing the adhesion between the insulating layer and the metal layer, the glass transition temperature of the maleimide compound X is preferably 70° C. or higher, more preferably 80° C. or higher.
[0066] The glass transition temperature can be determined from the inflection point of the reverse heat flow when the material is heated in a nitrogen atmosphere from -30°C to 260°C at a heating rate of 3°C / min using a differential scanning calorimeter (e.g., TA Instruments' "Q2000").
[0067] In order to exert the effects of the present invention, the content of the maleimide compound X is 5% by weight or more in 100% by weight of the components excluding the inorganic filler and the solvent in the resin material.
[0068] In order to more effectively exert the effects of the present invention, the content of the maleimide compound X is preferably 10% by weight or more, preferably 80% by weight or less, and more preferably 70% by weight or less, based on 100% by weight of the components in the resin material excluding the inorganic filler and the solvent. When the content of the maleimide compound X is equal to or more than the lower limit, the dielectric tangent of the cured product can be further reduced.
[0069] [Curable compound] The resin material preferably contains a curable compound different from the maleimide compound X. The curable compounds may be used alone or in combination of two or more.
[0070] The curable compound may include a thermosetting compound and a photocurable compound. The curable compound may include only a thermosetting compound, may include only a photocurable compound, or may include a thermosetting compound and a photocurable compound. The curable compound may include a compound having both thermosetting and photocuring properties (thermo- and photocurable compound). The thermosetting compound may include a thermo- and photocurable compound.
[0071] The curable compound preferably contains a curable compound having a weight average molecular weight of less than 1500. In this case, the resin material can be cured well, and the effects of the present invention can be more effectively exhibited.
[0072] The weight average molecular weight of the curable compound is a weight average molecular weight measured by gel permeation chromatography (GPC) in terms of polystyrene.
[0073] The content of the heat- and light-curable compound in 100% by weight of the components in the resin material excluding the inorganic filler and the solvent is preferably 10% by weight or more, more preferably 20% by weight or more, even more preferably 30% by weight or more, preferably 90% by weight or less, and more preferably 80% by weight or less. When the content of the heat- and light-curable compound is equal to or more than the lower limit and equal to or less than the upper limit, the curing reaction can proceed sufficiently.
[0074] The content of the photocurable compound in 100% by weight of the components in the resin material excluding the inorganic filler and the solvent is preferably 10% by weight or more, more preferably 20% by weight or more, even more preferably 30% by weight or more, preferably 90% by weight or less, more preferably 80% by weight or less. When the content of the photocurable compound is equal to or more than the lower limit and equal to or less than the upper limit, the curing reaction can proceed sufficiently.
[0075] [Thermosetting compound] The resin material preferably contains a thermosetting compound different from the maleimide compound X. The thermosetting compounds may be used alone or in combination of two or more.
[0076] Examples of the thermosetting compound include a phenoxy compound, an oxetane compound, a maleimide compound different from the maleimide compound X (hereinafter, may be referred to as a maleimide compound Y), an epoxy compound, a cyanate compound, a vinyl compound, a polyarylate compound, a diallyl phthalate compound, an episulfide compound, a (meth)acrylic compound, an amino compound, an unsaturated polyester compound, a polyurethane compound, and a silicone compound.
[0077] The thermosetting compound is preferably a maleimide compound Y, an epoxy compound, or a vinyl compound, more preferably contains an epoxy compound or a vinyl compound, and even more preferably contains an epoxy compound. The vinyl compound preferably contains a styrene compound or an acrylate compound, and more preferably contains a styrene compound. In this case, the dielectric tangent of the cured product can be further lowered and the thermal dimensional stability of the cured product can be further improved.
[0078] <Maleimide compound Y> When a maleimide compound-containing liquid containing 5% by weight of the maleimide compound Y and 95% by weight of cyclohexanone (hereinafter sometimes referred to as "third maleimide compound-containing liquid") is obtained, the maleimide compound Y is a maleimide compound having the property that the cloudiness of the maleimide compound-containing liquid (third maleimide compound-containing liquid) is less than 5%. The maleimide compound Y is a maleimide compound different from the maleimide compound X. Only one type of the maleimide compound Y may be used, or two or more types may be used in combination.
[0079] The third maleimide compound-containing liquid is prepared in order to determine whether or not the maleimide compound Y has a specific property. In the resin material according to the present invention, the maleimide compound Y does not have to be added as a third maleimide compound-containing liquid containing 5% by weight of the maleimide compound Y and 95% by weight of cyclohexanone.
[0080] The maleimide compound Y may be a heat and light curable compound.
[0081] The maleimide compound Y may be a bismaleimide compound.
[0082] Examples of the maleimide compound Y include N-phenylbismaleimide and N-alkylbismaleimide.
[0083] The maleimide compound Y preferably has a skeleton derived from a diamine compound other than a dimer diamine or a triamine compound other than a trimer triamine.
[0084] The maleimide compound Y preferably has an aromatic skeleton.
[0085] In the maleimide compound Y, the nitrogen atom in the maleimide skeleton is preferably bonded to an aromatic ring.
[0086] From the viewpoint of further enhancing the thermal dimensional stability of the cured product, the content of the maleimide compound Y is preferably 0.5% by weight or more, more preferably 1% by weight or more, and preferably 15% by weight or less, more preferably 10% by weight or less, based on 100% by weight of the components excluding the solvent in the resin material.
[0087] In 100% by weight of the components in the resin material excluding the inorganic filler and the solvent, the content of the maleimide compound Y is preferably 2.5% by weight or more, more preferably 5% by weight or more, even more preferably 7.5% by weight or more, preferably 50% by weight or less, and more preferably 35% by weight or less. When the content of the maleimide compound Y is equal to or more than the lower limit and equal to or less than the upper limit, the thermal dimensional stability of the cured product can be further improved.
[0088] From the viewpoint of effectively exerting the effects of the present invention, the molecular weight of the maleimide compound Y is preferably 500 or more, more preferably 1000 or more, and preferably less than 30000, more preferably less than 20000. When a resin material containing the maleimide compound Y is photocured for use, from the viewpoint of effectively exerting the effects of the present invention, the molecular weight of the maleimide compound Y is preferably less than 3000, more preferably less than 1500, and even more preferably less than 1000.
[0089] The molecular weight of the maleimide compound Y means a molecular weight that can be calculated from the structural formula when the maleimide compound Y is not a polymer and when the structural formula of the maleimide compound can be specified. When the maleimide compound is a polymer, the molecular weight of the maleimide compound means a weight average molecular weight in terms of polystyrene measured by gel permeation chromatography (GPC).
[0090] Commercially available examples of the maleimide compound Y include "BMI-4000" and "BMI-5100" manufactured by Daiwa Chemical Industry Co., Ltd., "MIR-3000" manufactured by Nippon Kayaku Co., Ltd., and "BMI-1500" and "BMI-689" manufactured by Designer Molecules Inc.
[0091] <Epoxy compounds> As the epoxy compound, a conventionally known epoxy compound can be used. The epoxy compound is an organic compound having at least one epoxy group. The epoxy compound may be used alone or in combination of two or more kinds.
[0092] Examples of the epoxy compound include bisphenol A type epoxy compounds, bisphenol F type epoxy compounds, bisphenol S type epoxy compounds, phenol novolac type epoxy compounds, biphenyl type epoxy compounds, biphenyl novolac type epoxy compounds, biphenol type epoxy compounds, naphthalene type epoxy compounds, fluorene type epoxy compounds, phenol aralkyl type epoxy compounds, naphthol aralkyl type epoxy compounds, dicyclopentadiene type epoxy compounds, anthracene type epoxy compounds, epoxy compounds having an adamantane skeleton, epoxy compounds having a tricyclodecane skeleton, naphthylene ether type epoxy compounds, and epoxy compounds having a triazine nucleus in the skeleton.
[0093] The epoxy compound may be a glycidyl ether compound, which is a compound having at least one glycidyl ether group.
[0094] From the viewpoint of further lowering the dielectric tangent of the cured product and enhancing the thermal dimensional stability and flame retardancy of the cured product, the epoxy compound preferably contains an epoxy compound having an aromatic skeleton, preferably contains an epoxy compound having a naphthalene skeleton or a phenyl skeleton, and is more preferably an epoxy compound having an aromatic skeleton.
[0095] From the viewpoint of further lowering the dielectric tangent of the cured product and improving the coefficient of linear expansion (CTE) of the cured product, it is preferable that the epoxy compound contains an epoxy compound that is liquid at 25°C and an epoxy compound that is solid at 25°C.
[0096] The viscosity at 25°C of the epoxy compound that is liquid at 25°C is preferably 1000 mPa·s or less, and more preferably 500 mPa·s or less.
[0097] The viscosity of the epoxy compound can be measured, for example, using a dynamic viscoelasticity measuring device ("VAR-100" manufactured by Rheologica Instruments).
[0098] It is more preferable that the molecular weight of the epoxy compound is 1000 or less. In this case, even if the content of the inorganic filler is 50% by weight or more in 100% by weight of the components excluding the solvent in the resin material, a resin material having high fluidity during the formation of an insulating layer can be obtained. Therefore, when the uncured or B-staged resin material is laminated on a circuit board, the inorganic filler can be uniformly present.
[0099] The molecular weight of the epoxy compound means a molecular weight that can be calculated from the structural formula when the epoxy compound is not a polymer and when the structural formula of the epoxy compound can be specified, and means a weight average molecular weight when the epoxy compound is a polymer.
[0100] From the viewpoint of further enhancing the thermal dimensional stability of the cured product, the content of the above-mentioned epoxy compound is preferably 4 wt % or more, more preferably 7 wt % or more, and preferably 15 wt % or less, more preferably 12 wt % or less, based on 100 wt % of the components excluding the solvent in the resin material.
[0101] The content of the epoxy compound is preferably 15% by weight or more, more preferably 25% by weight or more, and preferably 50% by weight or less, more preferably 40% by weight or less, based on 100% by weight of the components in the resin material excluding the inorganic filler and the solvent. When the content of the epoxy compound is equal to or more than the lower limit and equal to or less than the upper limit, the thermal dimensional stability of the cured product can be further improved.
[0102] The weight ratio of the content of the epoxy compound to the total content of the maleimide compound X and a curing agent described later (the content of the epoxy compound / the total content of the maleimide compound X and a curing agent described later) is preferably 0.2 or more, more preferably 0.3 or more, and preferably 1 or less, more preferably 0.8 or less. When the weight ratio is equal to or more than the lower limit and equal to or less than the upper limit, the dielectric tangent can be further lowered and the thermal dimensional stability can be further improved.
[0103] <Vinyl compounds> As the vinyl compound, a conventionally known vinyl compound can be used. The vinyl compound is an organic compound having at least one vinyl group. The vinyl compound may be used alone or in combination of two or more kinds.
[0104] The vinyl compound may be a styrene compound, an acrylate compound, a divinyl compound, or the like. The divinyl compound may be a divinyl benzyl ether compound. The vinyl compound may be a divinyl compound having an aliphatic skeleton, or a divinyl ether compound. The acrylate compound may be a heat-curable or photocurable compound.
[0105] The styrene compound may be a phenylene ether compound modified with a terminal styrene. The styrene compound may be used alone or in combination of two or more kinds.
[0106] An example of a commercially available styrene compound is "OPE-2St" manufactured by Mitsubishi Gas Chemical Company, Inc.
[0107] The content of the vinyl compound in 100% by weight of the components in the resin material excluding the inorganic filler and the solvent is preferably 5% by weight or more, more preferably 10% by weight or more, even more preferably 20% by weight or more, preferably 80% by weight or less, and more preferably 70% by weight or less. When the content of the vinyl compound is equal to or more than the lower limit and equal to or less than the upper limit, the thermal dimensional stability of the cured product can be further improved.
[0108] [Inorganic filler] The resin material preferably contains an inorganic filler. By using the inorganic filler, the dielectric tangent of the cured product can be further reduced. In addition, by using the inorganic filler, the dimensional change of the cured product due to heat can be further reduced. The inorganic filler may be used alone or in combination of two or more kinds.
[0109] Examples of the inorganic filler include silica, talc, clay, mica, hydrotalcite, alumina, magnesium oxide, aluminum hydroxide, diamond, aluminum nitride, and boron nitride.
[0110] The inorganic filler is preferably an inorganic filler having a thermal conductivity of 10 W / mK or more, such as alumina or boron nitride, which can enhance heat dissipation.
[0111] From the viewpoint of reducing the surface roughness of the cured product, further increasing the adhesive strength between the cured product and the metal layer, forming finer wiring on the surface of the cured product, and imparting better insulation reliability to the cured product, the inorganic filler is preferably silica or alumina, more preferably silica, and even more preferably fused silica. The silica may be hollow silica. By using silica, the thermal expansion coefficient of the cured product is further reduced, and the dielectric tangent of the cured product is further reduced. In addition, by using silica, the surface roughness of the cured product is effectively reduced, and the adhesive strength between the cured product and the metal layer is effectively increased. The shape of the silica is preferably spherical.
[0112] From the viewpoints of promoting resin curing regardless of the curing environment, effectively increasing the glass transition temperature of the cured product, and effectively reducing the coefficient of linear thermal expansion of the cured product, it is preferable that the inorganic filler be spherical silica.
[0113] From the viewpoint of increasing the thermal conductivity and the insulating property, the inorganic filler is preferably alumina or boron nitride. In particular, boron nitride has anisotropy, and therefore can further reduce the coefficient of linear thermal expansion.
[0114] The inorganic filler has an average particle size of preferably 50 nm or more, more preferably 100 nm or more, even more preferably 500 nm or more, and preferably 5 μm or less, more preferably 3 μm or less, and even more preferably 1 μm or less. When the inorganic filler has an average particle size of not less than the lower limit and not more than the upper limit, the surface roughness after etching can be reduced and the plating peel strength can be increased, and the adhesion between the insulating layer and the metal layer can be further improved.
[0115] The median diameter (d50) at 50% is used as the average particle diameter of the inorganic filler. The average particle diameter can be measured using a particle size distribution measuring device using a laser diffraction scattering method. In addition, when the inorganic filler is an aggregated particle, the average particle diameter of the inorganic filler means the primary particle diameter.
[0116] The inorganic filler is preferably spherical, more preferably spherical silica. In this case, the surface roughness of the cured product is effectively reduced, and the adhesive strength between the cured product and the metal layer is effectively increased. When the inorganic filler is spherical, the aspect ratio of the inorganic filler is preferably 2 or less, more preferably 1.5 or less.
[0117] The inorganic filler is preferably surface-treated, more preferably surface-treated with a coupling agent, and even more preferably surface-treated with a silane coupling agent.By surface-treating the inorganic filler, the surface roughness of the roughened cured product is further reduced, and the adhesive strength between the cured product and the metal layer is further increased.In addition, by surface-treating the inorganic filler, finer wiring can be formed on the surface of the cured product, and better inter-wiring insulation reliability and inter-layer insulation reliability can be imparted to the cured product.
[0118] The coupling agent includes a silane coupling agent, a titanium coupling agent, an aluminum coupling agent, etc. The silane coupling agent includes a methacrylsilane, an acrylsilane, an aminosilane, an imidazole silane, a vinylsilane, an epoxysilane, etc.
[0119] The content of the inorganic filler in 100% by weight of the resin material excluding the solvent is preferably 50% by weight or more, more preferably 60% by weight or more, even more preferably 65% by weight or more, particularly preferably 68% by weight or more, preferably 90% by weight or less, more preferably 85% by weight or less, even more preferably 80% by weight or less, particularly preferably 75% by weight or less. When the content of the inorganic filler is equal to or more than the lower limit, the dielectric loss tangent is effectively lowered. When the content of the inorganic filler is equal to or less than the upper limit, the thermal dimensional stability is improved and the warping of the cured product can be effectively suppressed. When the content of the inorganic filler is equal to or more than the lower limit and equal to or less than the upper limit, the surface roughness of the cured product can be further reduced, and finer wiring can be formed on the surface of the cured product. Furthermore, with this content of the inorganic filler, it is possible to lower the thermal expansion coefficient of the cured product and at the same time improve the smear removability.
[0120] [Hardening agent] The resin material preferably contains a curing agent. The curing agent is not particularly limited. A conventionally known curing agent can be used as the curing agent. The curing agent may be used alone or in combination of two or more kinds.
[0121] Examples of the curing agent include a phenol compound (phenol curing agent), an active ester compound, a cyanate ester compound (cyanate ester curing agent), a benzoxazine compound (benzoxazine curing agent), a carbodiimide compound (carbodiimide curing agent), an amine compound (amine curing agent), a thiol compound (thiol curing agent), a phosphine compound, a dicyandiamide, and an acid anhydride. The curing agent preferably has a functional group capable of reacting with the epoxy group of the epoxy compound.
[0122] From the viewpoint of further increasing the thermal dimensional stability, the curing agent preferably contains at least one component selected from the group consisting of a phenolic compound, an active ester compound, a cyanate ester compound, a benzoxazine compound, a carbodiimide compound, and an acid anhydride. From the viewpoint of further increasing the thermal dimensional stability, the curing agent more preferably contains at least one component selected from the group consisting of a phenolic compound, an active ester compound, a cyanate ester compound, a benzoxazine compound, and a carbodiimide compound, and further preferably contains an active ester compound.
[0123] From the viewpoint of further enhancing the thermal dimensional stability, it is preferable that the thermosetting compound contains an epoxy compound, and the curing agent contains both a phenol compound and an active ester compound.
[0124] Examples of the phenol compound include novolak type phenols, biphenol type phenols, naphthalene type phenols, dicyclopentadiene type phenols, aralkyl type phenols, and dicyclopentadiene type phenols.
[0125] Commercially available phenol compounds include novolac phenols ("TD-2091" manufactured by DIC Corporation), biphenyl novolac phenols ("MEH-7851" manufactured by Meiwa Kasei Co., Ltd.), aralkyl phenol compounds ("MEH-7800" manufactured by Meiwa Kasei Co., Ltd.), and phenols having an aminotriazine skeleton ("LA-1356" and "LA-3018-50P" manufactured by DIC Corporation).
[0126] The above-mentioned active ester compound refers to a compound that contains at least one ester bond in the structure and has an aliphatic chain, an aliphatic ring, or an aromatic ring bonded to both sides of the ester bond. The active ester compound is obtained, for example, by a condensation reaction between a carboxylic acid compound or a thiocarboxylic acid compound and a hydroxy compound or a thiol compound. An example of the active ester compound is a compound represented by the following formula (1).
[0127] [ka]
[0128] In the above formula (1), X1 represents a group containing an aliphatic chain, a group containing an aliphatic ring, or a group containing an aromatic ring, and X2 represents a group containing an aromatic ring. Preferred examples of the group containing an aromatic ring include a benzene ring which may have a substituent, and a naphthalene ring which may have a substituent. Examples of the substituent include a hydrocarbon group. The number of carbon atoms in the hydrocarbon group is preferably 12 or less, more preferably 6 or less, and even more preferably 4 or less.
[0129] In the above formula (1), the combination of X1 and X2 includes a combination of an optionally substituted benzene ring and an optionally substituted benzene ring, and a combination of an optionally substituted benzene ring and an optionally substituted naphthalene ring. Furthermore, in the above formula (1), the combination of X1 and X2 includes a combination of an optionally substituted naphthalene ring and an optionally substituted naphthalene ring.
[0130] The active ester compound is not particularly limited. From the viewpoint of further improving thermal dimensional stability and flame retardancy, the active ester compound is preferably an active ester compound having two or more aromatic skeletons. From the viewpoint of lowering the dielectric tangent of the cured product and improving the thermal dimensional stability of the cured product, the active ester compound more preferably has a naphthalene ring or a dicyclopentadiene skeleton in the main chain skeleton.
[0131] Commercially available products of the above active ester compound include "HPC-8000-65T", "EXB9416-70BK", "HPC-8150-62T", "EXB-8" and "EXB8100-65T" manufactured by DIC Corporation.
[0132] From the viewpoint of lowering the melt viscosity of the resin material, shortening the distance between crosslinking points, and further reducing the linear expansion coefficient of the cured product, the active ester compound is preferably an ester compound having low molecular weight activity. Commercially available ester compounds having low molecular weight activity include the above-mentioned "EXB-8" manufactured by DIC Corporation.
[0133] Examples of the cyanate ester compound include novolac-type cyanate ester resins, bisphenol-type cyanate ester resins, and prepolymers obtained by partially trimerizing these. Examples of the novolac-type cyanate ester resins include phenol novolac-type cyanate ester resins and alkylphenol-type cyanate ester resins. Examples of the bisphenol-type cyanate ester resins include bisphenol A-type cyanate ester resins, bisphenol E-type cyanate ester resins, and tetramethylbisphenol F-type cyanate ester resins.
[0134] Commercially available products of the cyanate ester compound include phenol novolac type cyanate ester resins ("PT-30" and "PT-60" manufactured by Lonza Japan) and prepolymers in which bisphenol type cyanate ester resins are trimerized ("BA-230S", "BA-3000S", "BTP-1000S" and "BTP-6020S" manufactured by Lonza Japan).
[0135] The content of the cyanate ester compound in 100% by weight of the components in the resin material excluding the inorganic filler and the solvent is preferably 10% by weight or more, more preferably 15% by weight or more, even more preferably 20% by weight or more, and preferably 85% by weight or less, more preferably 75% by weight or less. When the content of the cyanate ester compound is equal to or more than the lower limit and equal to or less than the upper limit, the thermal dimensional stability of the cured product can be further improved.
[0136] Examples of the benzoxazine compound include Pd-type benzoxazine and Fa-type benzoxazine.
[0137] Commercially available products of the above benzoxazine compound include "Pd type" manufactured by Shikoku Chemical Industry Co., Ltd. and "ODA-BOZ" manufactured by JFE Chemical Corporation.
[0138] The content of the benzoxazine compound in 100% by weight of the components in the resin material excluding the inorganic filler and the solvent is preferably 1% by weight or more, more preferably 5% by weight or more, even more preferably 10% by weight or more, preferably 70% by weight or less, more preferably 60% by weight or less. When the content of the benzoxazine compound is equal to or more than the lower limit and equal to or less than the upper limit, the dielectric tangent of the cured product can be lowered and the thermal dimensional stability can be further improved.
[0139] The carbodiimide compound is a compound having a structural unit represented by the following formula (2). In the following formula (2), the right end and the left end are bonding sites with other groups. The above carbodiimide compounds may be used alone or in combination of two or more kinds.
[0140] [ka]
[0141] In the above formula (2), X represents an alkylene group, a group in which a substituent is bonded to an alkylene group, a cycloalkylene group, a group in which a substituent is bonded to a cycloalkylene group, an arylene group, or a group in which a substituent is bonded to an arylene group, and p represents an integer of 1 to 5. When a plurality of Xs are present, the plurality of Xs may be the same or different.
[0142] In one preferred embodiment, at least one X is an alkylene group, a group in which a substituent is bonded to an alkylene group, a cycloalkylene group, or a group in which a substituent is bonded to a cycloalkylene group.
[0143] Commercially available examples of the carbodiimide compound include "Carbodilite V-02B", "Carbodilite V-03", "Carbodilite V-04K", "Carbodilite V-07", "Carbodilite V-09", "Carbodilite 10M-SP", and "Carbodilite 10M-SP (modified)" manufactured by Nisshinbo Chemical Inc., as well as "Stavaxol P", "Stavaxol P400", and "Hi-Kasil 510" manufactured by Rhein Chemie.
[0144] Examples of the acid anhydride include tetrahydrophthalic anhydride and alkylstyrene-maleic anhydride copolymer.
[0145] Commercially available products of the above acid anhydrides include "Rikacid TDA-100" manufactured by New Japan Chemical Co., Ltd.
[0146] The content of the curing agent relative to 100 parts by weight of the epoxy compound is preferably 70 parts by weight or more, more preferably 85 parts by weight or more, and preferably 150 parts by weight or less, and more preferably 120 parts by weight or less. When the content of the curing agent is equal to or more than the lower limit and equal to or less than the upper limit, the curing property is more excellent, the thermal dimensional stability is more improved, and the volatilization of the remaining unreacted components can be more suppressed.
[0147] In 100% by weight of the components in the resin material excluding the inorganic filler and the solvent, the total content of the maleimide compound X, the thermosetting compound, and the curing agent is preferably 50% by weight or more, more preferably 60% by weight or more, and preferably 98% by weight or less, more preferably 95% by weight or less. When the total content of the maleimide compound X, the thermosetting compound, and the curing agent is equal to or more than the lower limit and equal to or less than the upper limit, the curability is more excellent and the thermal dimensional stability can be further improved.
[0148] [Cure accelerator] The resin material includes a curing accelerator. The use of the curing accelerator further accelerates the curing speed. By quickly curing the resin material, the crosslinked structure in the cured product becomes uniform, and the number of unreacted functional groups decreases, resulting in a high crosslink density. The curing accelerator is not particularly limited, and conventionally known curing accelerators can be used. The curing accelerator may be used alone or in combination of two or more.
[0149] Examples of the curing accelerator include anionic curing accelerators such as imidazole compounds, cationic curing accelerators such as amine compounds, curing accelerators other than anionic and cationic curing accelerators such as phosphorus compounds and organometallic compounds, and radical curing accelerators such as peroxides.
[0150] Examples of the imidazole compound include 2-undecylimidazole, 2-heptadecylimidazole, 2-methylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, 1-benzyl-2-phenylimidazole, 1,2-dimethylimidazole, 1-cyanoethyl-2-methylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazolium trimellitate, and 1-cyanoethyl-2-phenylimidazolium trimethylolate. remellitate, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-undecylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct, 2-phenylimidazole isocyanuric acid adduct, 2-methylimidazole isocyanuric acid adduct, 2-phenyl-4,5-dihydroxymethylimidazole, and 2-phenyl-4-methyl-5-dihydroxymethylimidazole.
[0151] Examples of the amine compound include diethylamine, triethylamine, diethylenetetramine, triethylenetetramine, and 4,4-dimethylaminopyridine.
[0152] The phosphorus compound includes a triphenylphosphine compound.
[0153] Examples of the organometallic compound include zinc naphthenate, cobalt naphthenate, tin octoate, cobalt octoate, cobalt bisacetylacetonate (II), and cobalt trisacetylacetonate (III).
[0154] The peroxides include dicumyl peroxide and Perhexyl 25B.
[0155] From the viewpoint of further reducing the curing temperature and effectively suppressing warping of the cured product, the curing accelerator preferably contains the anionic curing accelerator, and more preferably contains the imidazole compound.
[0156] From the viewpoint of further suppressing the curing temperature and effectively suppressing warping of the cured product, the content of the anionic curing accelerator in 100% by weight of the curing accelerator is preferably 20% by weight or more, more preferably 50% by weight or more, even more preferably 70% by weight or more, and most preferably 100% by weight (total amount). Therefore, it is most preferable that the curing accelerator is the anionic curing accelerator.
[0157] When the thermosetting compound contains a radically curable compound such as the vinyl compound, the acrylate compound, or the styrene compound, radical curing proceeds, so that the curing accelerator preferably contains the radical curing accelerator.
[0158] The curing accelerator preferably includes a photocuring accelerator. When the resin material includes the heat- and photocurable compound or the photocurable compound, the curing accelerator preferably includes a photocuring accelerator.
[0159] From the viewpoint of enhancing reactivity, the photocuring accelerator is preferably a photocuring accelerator whose absorption wavelength is greater than or does not overlap with the absorption wavelength of the maleimide compound Y.
[0160] The content of the curing accelerator is not particularly limited. In 100% by weight of the components in the resin material excluding the inorganic filler and the solvent, the content of the curing accelerator is preferably 0.01% by weight or more, more preferably 0.05% by weight or more, preferably 5% by weight or less, more preferably 3% by weight or less. When the content of the curing accelerator is equal to or more than the lower limit and equal to or less than the upper limit, the resin material is cured efficiently. When the content of the curing accelerator is within a more preferred range, the storage stability of the resin material is further increased, and a better cured product is obtained.
[0161] [Thermoplastic resin] The resin material preferably contains a thermoplastic resin. Examples of the thermoplastic resin include polyvinyl acetal resin, polyimide resin, phenoxy resin, and styrene-butadiene resin. The thermoplastic resin may be used alone or in combination of two or more.
[0162] From the viewpoint of effectively lowering the dielectric tangent and effectively increasing the adhesion of the metal wiring regardless of the curing environment, the thermoplastic resin is preferably a phenoxy resin. By using the phenoxy resin, the deterioration of the embedding ability of the resin film in the holes or irregularities of the circuit board and the non-uniformity of the inorganic filler are suppressed. In addition, by using the phenoxy resin, the melt viscosity can be adjusted, so that the dispersibility of the inorganic filler is improved, and the resin composition or the B-stage product is less likely to wet and spread to unintended areas during the curing process.
[0163] The phenoxy resin contained in the resin material is not particularly limited. As the phenoxy resin, a conventionally known phenoxy resin can be used. The phenoxy resin may be used alone or in combination of two or more kinds.
[0164] Examples of the phenoxy resin include phenoxy resins having a skeleton such as a bisphenol A skeleton, a bisphenol F skeleton, a bisphenol S skeleton, a biphenyl skeleton, a novolac skeleton, a naphthalene skeleton, and an imide skeleton.
[0165] Commercially available examples of the phenoxy resin include "YP50", "YP55", and "YP70" manufactured by Nippon Steel & Sumikin Chemical Co., Ltd., and "1256B40", "4250", "4256H40", "4275", "YX6954BH30", and "YX8100BH30" manufactured by Mitsubishi Chemical Corporation.
[0166] From the viewpoints of improving handleability, plating peel strength at low roughness, and adhesion between the insulating layer and the metal layer, the thermoplastic resin is preferably a polyimide resin (polyimide compound).
[0167] From the viewpoint of improving solubility, the polyimide compound is preferably a polyimide compound obtained by a method of reacting a tetracarboxylic dianhydride with a dimer diamine.
[0168] Examples of the tetracarboxylic dianhydride include pyromellitic dianhydride, 3,3',4,4'-benzophenone tetracarboxylic dianhydride, 3,3',4,4'-biphenylsulfone tetracarboxylic dianhydride, 1,4,5,8-naphthalene tetracarboxylic dianhydride, 2,3,6,7-naphthalene tetracarboxylic dianhydride, 3,3',4,4'-biphenyl ether tetracarboxylic dianhydride, 3,3',4,4'-dimethyldiphenylsilane tetracarboxylic dianhydride, 3,3',4,4'-tetraphenylsilane tetracarboxylic dianhydride, 1,2,3,4-furan tetracarboxylic dianhydride, 4,4'-bis(3,4-dicarboxyphenoxy)diphenylsulfonate, and 4,4'-bis(3,4-dicarboxyphenoxy)diphenylsulfonate. sulfide dianhydride, 4,4'-bis(3,4-dicarboxyphenoxy)diphenylsulfone dianhydride, 4,4'-bis(3,4-dicarboxyphenoxy)diphenylpropane dianhydride, 3,3',4,4'-perfluoroisopropylidenediphthalic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, bis(phthalic acid)phenylphosphine oxide dianhydride, p-phenylene-bis(triphenylphthalic acid) dianhydride, m-phenylene-bis(triphenylphthalic acid) dianhydride, bis(triphenylphthalic acid)-4,4'-diphenyl ether dianhydride, and bis(triphenylphthalic acid)-4,4'-diphenylmethane dianhydride.
[0169] Examples of the dimer diamine include VERSAMINE 551 (trade name, manufactured by BASF Japan, 3,4-bis(1-aminoheptyl)-6-hexyl-5-(1-octenyl)cyclohexene), VERSAMINE 552 (trade name, manufactured by Cognics Japan, hydrogenated VERSAMINE 551), PRIAMINE 1075, and PRIAMINE 1074 (trade names, all manufactured by Croda Japan).
[0170] The polyimide compound may have an acid anhydride structure, a maleimide structure, or a citraconic imide structure at the end. In this case, the polyimide compound can be reacted with an epoxy resin. By reacting the polyimide compound with an epoxy compound, the thermal dimensional stability of the cured product can be improved.
[0171] From the viewpoint of obtaining a resin material having even better storage stability, the weight average molecular weight of the thermoplastic resin, the polyimide resin and the phenoxy resin is preferably 10,000 or more, more preferably 15,000 or more, even more preferably 20,000 or more, and preferably 100,000 or less, more preferably 50,000 or less.
[0172] The weight average molecular weights of the thermoplastic resin, the polyimide resin and the phenoxy resin indicate weight average molecular weights in terms of polystyrene measured by gel permeation chromatography (GPC).
[0173] The contents of the thermoplastic resin, the polyimide resin, and the phenoxy resin are not particularly limited. In 100% by weight of the components in the resin material excluding the inorganic filler and the solvent, the content of the thermoplastic resin (when the thermoplastic resin is a polyimide resin or a phenoxy resin, the content of the polyimide resin or the phenoxy resin) is preferably 1% by weight or more, more preferably 2% by weight or more, preferably 30% by weight or less, more preferably 20% by weight or less. When the content of the thermoplastic resin is equal to or more than the lower limit and equal to or less than the upper limit, the resin material has good embedding properties in holes or irregularities in a circuit board. When the content of the thermoplastic resin is equal to or more than the lower limit, the formation of a resin film becomes easier, and a better insulating layer is obtained. When the content of the thermoplastic resin is equal to or less than the upper limit, the thermal expansion coefficient of the cured product becomes even lower. When the content of the thermoplastic resin is equal to or less than the upper limit, the surface roughness of the surface of the cured product becomes even smaller, and the adhesive strength between the cured product and the metal layer becomes even higher.
[0174] [solvent] The resin material does not contain or contains a solvent. By using the solvent, the viscosity of the resin material can be controlled within a suitable range, and the coatability of the resin material can be improved. The solvent may be used to obtain a slurry containing the inorganic filler. The solvent may be used alone or in combination of two or more.
[0175] Examples of the solvent include acetone, methanol, ethanol, butanol, 2-propanol, 2-methoxyethanol, 2-ethoxyethanol, 1-methoxy-2-propanol, 2-acetoxy-1-methoxypropane, toluene, xylene, methyl ethyl ketone, N,N-dimethylformamide, methyl isobutyl ketone, N-methyl-pyrrolidone, n-hexane, cyclohexane, cyclohexanone, and naphtha, which is a mixture.
[0176] Most of the solvent is preferably removed when the resin composition is molded into a film. Therefore, the boiling point of the solvent is preferably 200°C or less, more preferably 180°C or less. The content of the solvent in the resin composition is not particularly limited. The content of the solvent can be appropriately changed in consideration of the coatability of the resin composition.
[0177] When the resin material is a B-stage film, the content of the solvent in 100% by weight of the B-stage film is preferably 1% by weight or more, more preferably 2% by weight or more, preferably 10% by weight or less, more preferably 5% by weight or less.
[0178] [Other ingredients] For the purpose of improving impact resistance, heat resistance, resin compatibility, workability, and the like, the resin material may contain an organic filler, a leveling agent, a flame retardant, a coupling agent, a colorant, an antioxidant, an ultraviolet degradation inhibitor, a defoaming agent, a thickener, a thixotropy imparting agent, and the like.
[0179] The organic filler may be a particulate material made of benzoxazine resin, benzoxazole resin, fluororesin, acrylic resin, styrene resin, or the like. The fluororesin may be polytetrafluoroethylene (PTFE), or the like. By using fluororesin particles as the organic filler, the relative dielectric constant of the cured product can be further reduced. The average particle size of the organic filler is preferably 1 μm or less. When the average particle size of the organic filler is equal to or less than the upper limit, the surface roughness after etching can be reduced and the plating peel strength can be increased, and the adhesion between the insulating layer and the metal layer can be further improved. The average particle size of the organic filler may be 50 nm or more.
[0180] The median diameter (d50) at 50% is used as the average particle diameter of the organic filler. The average particle diameter can be measured using a particle size distribution measuring device using a laser diffraction scattering method.
[0181] The coupling agent includes a silane coupling agent, a titanium coupling agent, an aluminum coupling agent, etc. The silane coupling agent includes a vinyl silane, an amino silane, an imidazole silane, an epoxy silane, etc.
[0182] (Resin film) The above-mentioned resin composition is molded into a film to obtain a resin film (B-stage product / B-stage film). The above-mentioned resin material is preferably a resin film. The resin film is preferably a B-stage film.
[0183] Examples of methods for forming a resin composition into a film to obtain a resin film include the following: an extrusion molding method in which a resin composition is melt-kneaded and extruded using an extruder, and then molded into a film using a T-die or a circular die; a casting molding method in which a resin composition containing a solvent is cast into a film; and other conventionally known film molding methods. The extrusion molding method and the casting molding method are preferred because they can be made thinner. Films include sheets.
[0184] The resin composition is molded into a film and dried by heating at, for example, 50° C. to 150° C. for 1 minute to 10 minutes to the extent that curing by heat does not proceed too much, to obtain a resin film that is a B-stage film.
[0185] The film-like resin composition obtained by the drying process as described above is called a B-stage film. The B-stage film is in a semi-cured state. The semi-cured product is not completely cured and can be further cured.
[0186] The resin film does not have to be a prepreg. When the resin film is not a prepreg, migration does not occur along the glass cloth, etc. In addition, when the resin film is laminated or precured, unevenness due to the glass cloth does not occur on the surface.
[0187] The resin film can be used in the form of a laminated film comprising a metal foil or a base film and a resin film laminated on the surface of the metal foil or the base film. The metal foil is preferably a copper foil.
[0188] Examples of the base film of the laminated film include polyester resin films such as polyethylene terephthalate film and polybutylene terephthalate film, olefin resin films such as polyethylene film and polypropylene film, and polyimide resin films. The surface of the base film may be subjected to a release treatment as necessary.
[0189] From the viewpoint of controlling the degree of cure of the resin film more uniformly, the thickness of the resin film is preferably 5 μm or more and preferably 200 μm or less. When the resin film is used as an insulating layer of a circuit, the thickness of the insulating layer formed by the resin film is preferably equal to or more than the thickness of the conductor layer (metal layer) forming the circuit. The thickness of the insulating layer is preferably 5 μm or more and preferably 200 μm or less.
[0190] (Semiconductor devices, printed wiring boards, copper-clad laminates and multi-layer printed wiring boards) The above-mentioned resin material is suitably used for forming a molding resin in which a semiconductor chip is embedded in a semiconductor device.
[0191] The resin material is preferably used as an insulating material, and is preferably used for forming an insulating layer in a printed wiring board.
[0192] The printed wiring board is obtained, for example, by hot-pressing and molding the resin material.
[0193] A laminated member having a metal layer on one or both sides can be laminated to the resin film. A laminated structure can be suitably obtained, which includes a laminated member having a metal layer on its surface and a resin film laminated on the surface of the metal layer, and the resin film is the above-mentioned resin material. The method for laminating the resin film and the laminated member having the metal layer on its surface is not particularly limited, and a known method can be used. For example, the resin film can be laminated to a laminated member having a metal layer on its surface while applying pressure with or without heating using a device such as a parallel plate press or a roll laminator.
[0194] The material of the metal layer is preferably copper.
[0195] The lamination target member having the metal layer on the surface thereof may be a metal foil such as a copper foil.
[0196] The resin material is preferably used to obtain a copper-clad laminate. An example of the copper-clad laminate is a copper-clad laminate including a copper foil and a resin film laminated on one surface of the copper foil.
[0197] The thickness of the copper foil of the copper-clad laminate is not particularly limited. The thickness of the copper foil is preferably within a range of 1 μm to 50 μm. In addition, in order to increase the adhesive strength between the cured product of the resin material and the copper foil, the copper foil preferably has fine irregularities on its surface. The method of forming the irregularities is not particularly limited. Examples of the method of forming the irregularities include a forming method by treatment using a known chemical solution.
[0198] The above resin materials are suitably used to obtain multi-layer substrates.
[0199] An example of the multilayer board is a multilayer board including a circuit board and an insulating layer laminated on the circuit board. The insulating layer of the multilayer board is formed of the resin material. The insulating layer of the multilayer board may be formed of the resin film of the laminate film by using a laminate film. The insulating layer is preferably laminated on the surface of the circuit board on which the circuit is provided. A part of the insulating layer is preferably embedded between the circuits.
[0200] In the multilayer board, the surface of the insulating layer opposite to the surface on which the circuit board is laminated is preferably roughened.
[0201] The roughening treatment method is not particularly limited and may be any conventionally known roughening treatment method. The surface of the insulating layer may be subjected to a swelling treatment before the roughening treatment.
[0202] Preferably, the multilayer substrate further comprises a copper plating layer laminated on the roughened surface of the insulating layer.
[0203] Another example of the multilayer board is a multilayer board comprising a circuit board, an insulating layer laminated on the surface of the circuit board, and a copper foil laminated on the surface of the insulating layer opposite to the surface on which the circuit board is laminated. The insulating layer is preferably formed by using a copper-clad laminate comprising copper foil and a resin film laminated on one surface of the copper foil, and curing the resin film. Furthermore, the copper foil is preferably etched to form a copper circuit.
[0204] Another example of the multilayer board is a multilayer board including a circuit board and a plurality of insulating layers laminated on a surface of the circuit board. At least one of the insulating layers arranged on the circuit board is formed using the resin material. The multilayer board preferably further includes a circuit laminated on at least one surface of the insulating layer formed using the resin film.
[0205] In the case of a multilayer printed wiring board among multilayer substrates, a low dielectric tangent and high insulation reliability due to an insulating layer are required, and therefore the resin material according to the present invention is suitably used for forming an insulating layer in the multilayer printed wiring board.
[0206] The multilayer printed wiring board includes, for example, a circuit board, a plurality of insulating layers disposed on a surface of the circuit board, and a metal layer disposed between the plurality of insulating layers, at least one of which is a cured product of the resin material.
[0207] FIG. 1 is a cross-sectional view that illustrates a multilayer printed wiring board that uses a resin material according to one embodiment of the present invention.
[0208] In the multilayer printed wiring board 11 shown in FIG. 1, a plurality of insulating layers 13-16 are laminated on the upper surface 12a of the circuit board 12. The insulating layers 13-16 are cured layers. A metal layer 17 is formed on a partial region of the upper surface 12a of the circuit board 12. Of the plurality of insulating layers 13-16, the insulating layers 13-15 other than the insulating layer 16 located on the outer surface opposite to the circuit board 12 side have the metal layer 17 formed on a partial region of the upper surface. The metal layer 17 is a circuit. The metal layer 17 is disposed between the circuit board 12 and the insulating layer 13, and between each of the laminated insulating layers 13-16. The lower metal layer 17 and the upper metal layer 17 are connected to each other by at least one of a via hole connection and a through hole connection not shown.
[0209] In the multilayer printed wiring board 11, the insulating layers 13-16 are formed of a cured product of the above-mentioned resin material. In this embodiment, the surfaces of the insulating layers 13-16 are roughened, so that fine holes (not shown) are formed on the surfaces of the insulating layers 13-16. The metal layer 17 reaches the inside of the fine holes. In the multilayer printed wiring board 11, the width dimension (L) of the metal layer 17 and the width dimension (S) of the portion where the metal layer 17 is not formed can be reduced. In the multilayer printed wiring board 11, good insulation reliability is provided between the upper metal layer and the lower metal layer that are not connected by via hole connection and through hole connection (not shown).
[0210] (Roughening treatment and swelling treatment) The resin material is preferably used to obtain a cured product to be subjected to roughening treatment or desmear treatment. The cured product also includes a pre-cured product that can be further cured.
[0211] In order to form fine irregularities on the surface of the cured product obtained by pre-curing the resin material, the cured product is preferably subjected to a roughening treatment. The cured product is preferably subjected to a swelling treatment before the roughening treatment. The cured product is preferably subjected to a swelling treatment after the pre-curing and before the roughening treatment, and is further preferably cured after the roughening treatment. However, the cured product does not necessarily have to be subjected to a swelling treatment.
[0212] As a method of the swelling treatment, for example, a method of treating the cured product with an aqueous solution or an organic solvent dispersion solution of a compound mainly composed of ethylene glycol or the like is used. The swelling liquid used in the swelling treatment generally contains an alkali as a pH adjuster or the like. The swelling liquid preferably contains sodium hydroxide. Specifically, for example, the swelling treatment is performed by treating the cured product with a 40 wt% ethylene glycol aqueous solution or the like at a treatment temperature of 30°C to 85°C for 1 minute to 30 minutes. The temperature of the swelling treatment is preferably within the range of 50°C to 85°C. If the temperature of the swelling treatment is too low, the swelling treatment takes a long time, and the adhesive strength between the cured product and the metal layer tends to be lowered.
[0213] In the roughening treatment, a chemical oxidizing agent such as a manganese compound, a chromium compound, or a persulfate compound is used. These chemical oxidizing agents are used as an aqueous solution or an organic solvent dispersion after water or an organic solvent is added. The roughening solution used in the roughening treatment generally contains an alkali as a pH adjuster. The roughening solution preferably contains sodium hydroxide.
[0214] The manganese compounds include potassium permanganate and sodium permanganate. The chromium compounds include potassium dichromate and potassium chromate anhydride. The persulfate compounds include sodium persulfate, potassium persulfate, and ammonium persulfate.
[0215] The arithmetic mean roughness Ra of the surface of the cured product is preferably 10 nm or more, preferably less than 300 nm, more preferably less than 200 nm, and even more preferably less than 150 nm. In this case, the adhesive strength between the cured product and the metal layer is increased, and finer wiring is formed on the surface of the insulating layer. Furthermore, conductor loss can be suppressed, and signal loss can be suppressed. The arithmetic mean roughness Ra is measured in accordance with JIS B0601:1994.
[0216] (Desmear processing) A through hole may be formed in the cured product obtained by pre-curing the resin material. In the multilayer board, etc., a via or a through hole is formed as the through hole. For example, a via can be formed by irradiating a laser such as a CO2 laser. The diameter of the via is not particularly limited, but is about 60 μm to 80 μm. Due to the formation of the through hole, a smear, which is a resin residue derived from the resin component contained in the cured product, is often formed at the bottom of the via.
[0217] In order to remove the smears, the surface of the cured product is preferably subjected to a desmear treatment. The desmear treatment may also serve as a roughening treatment.
[0218] In the desmear treatment, a chemical oxidizing agent such as a manganese compound, a chromium compound, or a persulfate compound is used, as in the roughening treatment. These chemical oxidizing agents are used as an aqueous solution or an organic solvent dispersion after water or an organic solvent is added. The desmear treatment liquid used in the desmear treatment generally contains an alkali. The desmear treatment liquid preferably contains sodium hydroxide.
[0219] By using the above resin material, the surface roughness of the surface of the cured product after the desmear treatment is sufficiently small.
[0220] The present invention will be specifically described below by way of examples and comparative examples, but the present invention is not limited to the following examples.
[0221] The following materials were prepared:
[0222] (Maleimide Compound X) Maleimide compound X-1: According to the following Synthesis Example 1, a maleimide compound X-1 (molecular weight 12000) represented by the following formula (X-1) was synthesized.
[0223] <Synthesis Example 1> In a 500 mL eggplant flask, 105 g of toluene, 41 g of N-methyl-2-pyrrolidone (NMP), and 7 g of methanesulfonic acid were placed. Then, 9.3 g (23 mmol) of dimer diamine ("PRIAMINE 1075" manufactured by Croda Japan) and 10.2 g (53 mmol) of tricyclodecane diamine were added. Then, 13.1 g (60 mmol) of pyromellitic dianhydride was added little by little. The eggplant flask was attached to a Dean-Stark apparatus and heated under reflux for 3.5 hours. In this way, a compound having amines at both ends and multiple imide skeletons was obtained. After removing the moisture discharged during condensation and returning to room temperature, 4.42 g (45 mmol) of maleic anhydride was added and stirred, and similarly heated and reacted. In this way, a compound having maleimide skeletons at both ends was obtained. The organic layer was washed with a mixed solvent of water and ethanol, and the mixed solvent was removed with an evaporator to obtain a toluene solution. Next, isopropanol was added to the toluene solution to reprecipitate the product. The product was then dried in a vacuum oven to obtain maleimide compound X-1. The structure represented by the following formula (X-1) is an example of maleimide compound X-1. Maleimide compound X-1 is, for example, a mixture containing a compound having a structure in which the position of the amino group is different from that of the structure represented by the following formula (X-1).
[0224] [ka]
[0225] Maleimide compound X-2: According to the following Synthesis Example 2, a maleimide compound X-2 (molecular weight 3300) was synthesized.
[0226] <Synthesis Example 2> In a 500 mL eggplant flask, 90 g of toluene, 46 g of N-methyl-2-pyrrolidone (NMP), and 9 g of methanesulfonic acid were added. Then, 15.6 g (80 mmol) of tricyclodecanediamine was added. Then, 13.1 g (60 mmol) of pyromellitic dianhydride was added little by little. Then, the eggplant flask was attached to a Dean-Stark apparatus and heated under reflux for 3.5 hours. In this way, a compound having an acid anhydride structure at the end and multiple imide skeletons was obtained. After removing the moisture discharged during condensation and returning to room temperature, 4.42 g (45 mmol) of maleic anhydride was added and stirred, and similarly heated to react. Next, the organic layer was washed with a mixed solvent of water and ethanol, and the mixed solvent was removed with an evaporator to obtain a toluene solution. Next, isopropanol was added to the toluene solution to re-precipitate the product. After that, it was dried in a vacuum oven to obtain maleimide compound X-2.
[0227] The molecular weight of the maleimide compound X synthesized in Synthesis Examples 1 and 2 was determined as follows.
[0228] GPC (Gel Permeation Chromatography) Measurement: The measurements were performed using a Shimadzu high-performance liquid chromatograph system, with tetrahydrofuran (THF) as the developing medium, at a column temperature of 40°C and a flow rate of 1.0 ml / min. The detector used was an SPD-10A, and two Shodex KF-804L columns (with an exclusion limit of 400,000) were connected in series. Tosoh TSK Standard Polystyrene was used as the standard polystyrene, and a calibration curve was created using substances with weight-average molecular weights Mw = 354,000, 189,000, 98,900, 37,200, 17,100, 9,830, 5,870, 2,500, 1,050, and 500, and the molecular weights were calculated.
[0229] (thermosetting compound) Maleimide compound Y-1: According to the following Synthesis Example 3, a maleimide compound Y-1 (molecular weight 17,500) was synthesized.
[0230] <Synthesis Example 3> In a 500 mL eggplant flask, 105 g of toluene, 41 g of N-methyl-2-pyrrolidone (NMP), and 7 g of methanesulfonic acid were added. 15.5 g (80 mmol) of tricyclodecanediamine and 32.8 g (80 mmol) of dimer diamine (PRIAMINE 1075 manufactured by Croda Japan) were added. Then, 62.5 g (120 mmol) of 4,4'-(4,4'-isopropylidenediphenoxy)diphthalic anhydride were added little by little. Next, the eggplant flask was attached to a Dean-Stark apparatus and heated under reflux for 3.5 hours. In this way, a compound having an acid anhydride structure at the terminal and multiple imide skeletons was obtained. After removing the moisture discharged during condensation and returning to room temperature, 8.83 g (90 mmol) of maleic anhydride was added and stirred, and similarly heated to react. The organic layer was then washed with a mixed solvent of water and ethanol, and the mixed solvent was removed using an evaporator to obtain a toluene solution. Isopropanol was then added to the toluene solution to reprecipitate the product. The product was then dried in a vacuum oven to obtain maleimide compound Y-1.
[0231] N-alkylbismaleimide compound (Designer Molecules Inc.'s "BMI-1500", maleimide compound Y) Biphenyl-type epoxy compound ("NC-3000" manufactured by Nippon Kayaku Co., Ltd.) Naphthalene-type epoxy compound ("ESN-475V" manufactured by Nippon Steel & Sumikin Chemical Co., Ltd.) Resorcinol diglycidyl ether (Nagase Chemtex Corporation "EX-201") Hyperbranched aliphatic epoxy compound (Nissan Chemical's "FoldiE101")
[0232] (Inorganic filler) Silica-containing slurry (75% silica by weight: Admatechs "SC4050-HOA", average particle size 1.0 μm, aminosilane treatment, cyclohexanone 25% by weight)
[0233] (hardening agent) Active ester compound 1-containing liquid (DIC Corporation "EXB-9416-70BK", solid content 70% by weight) Active ester compound 2-containing liquid (DIC Corporation "HPC-8150-62T", solid content 62% by weight) Phenol compound-containing liquid (DIC "LA-1356", solid content 60% by weight)
[0234] (Cure accelerator) Dimethylaminopyridine ("DMAP" manufactured by Wako Pure Chemical Industries, Ltd.) 2-Phenyl-4-methylimidazole ("2P4MZ" manufactured by Shikoku Chemical Industry Co., Ltd., anionic curing accelerator)
[0235] (thermoplastic resin) Polyimide compounds (polyimide resins): A solution containing a polyimide compound (non-volatile content: 26.8% by weight), which is a reaction product of tetracarboxylic dianhydride and dimer diamine, was synthesized according to Synthesis Example 4 below.
[0236] <Synthesis Example 4> In a reaction vessel equipped with a stirrer, a water divider, a thermometer, and a nitrogen gas inlet tube, 300.0 g of tetracarboxylic dianhydride ("BisDA-1000" manufactured by SABIC Japan LLC) and 665.5 g of cyclohexanone were placed, and the solution in the reaction vessel was heated to 60°C. Next, 89.0 g of dimer diamine ("PRIAMINE1075" manufactured by Croda Japan) and 54.7 g of 1,3-bisaminomethylcyclohexane (manufactured by Mitsubishi Gas Chemical Co., Ltd.) were dropped into the reaction vessel. Next, 121.0 g of methylcyclohexane and 423.5 g of ethylene glycol dimethyl ether were added to the reaction vessel, and the imidization reaction was carried out at 140°C for 10 hours. In this way, a polyimide compound-containing solution (non-volatile content 26.8% by weight) was obtained. The molecular weight (weight average molecular weight) of the obtained polyimide compound was 20,000. The molar ratio of acid component / amine component was 1.04.
[0237] The molecular weight of the polyimide compound synthesized in Synthesis Example 4 was determined as follows.
[0238] GPC (Gel Permeation Chromatography) Measurement: The measurements were performed using a Shimadzu high-performance liquid chromatograph system, with tetrahydrofuran (THF) as the developing medium, at a column temperature of 40°C and a flow rate of 1.0 ml / min. The detector used was an SPD-10A, and two Shodex KF-804L columns (with an exclusion limit of 400,000) were connected in series. Tosoh TSK Standard Polystyrene was used as the standard polystyrene, and a calibration curve was created using substances with weight-average molecular weights Mw = 354,000, 189,000, 98,900, 37,200, 17,100, 9,830, 5,870, 2,500, 1,050, and 500, and the molecular weights were calculated.
[0239] Example 1 , reference example 2 and Comparative Examples 1 and 2) The components shown in Table 1 below were mixed in the amounts (unit: parts by weight of solid content) shown in Table 1 below, and stirred at room temperature until a homogeneous solution was obtained, to obtain a resin material.
[0240] Preparation of resin film: The obtained resin material was applied to the release-treated surface of a release-treated PET film (Toray Industries, Inc., "XG284", thickness 25 μm) using an applicator, and then dried for 2 minutes and 30 seconds in a gear oven at 100°C to volatilize the solvent. In this way, a laminated film (a laminated film of a PET film and a resin film) was obtained in which a resin film (B-stage film) with a thickness of 40 μm was laminated on the PET film.
[0241] (evaluation) (1) Cloudiness of a liquid containing a maleimide compound A first maleimide compound-containing liquid was prepared by mixing 5% by weight of maleimide compounds (maleimide compound X-1, maleimide compound X-2, maleimide compound Y-1, N-alkyl bismaleimide compounds) with 95% by weight of cyclohexanone and thoroughly stirring the mixture. A second maleimide compound-containing liquid was prepared by mixing 10% by weight of maleimide compounds (maleimide compound X-1, maleimide compound X-2, maleimide compound Y-1, N-alkyl bismaleimide compounds) with 90% by weight of cyclohexanone and thoroughly stirring the mixture.
[0242] The first and second maleimide compound-containing liquids thus obtained were placed in a quartz cell (optical path length 1 cm), which was then placed in a haze meter ("HM-150" manufactured by Murakami Color Research Laboratory) to measure the haze.
[0243] (2) Ability to embed into uneven surfaces and prevent excessive wetting and spreading (prevention of overflow) Only the copper foil of a 100 mm square copper-clad laminate (a laminate of a 400 μm thick glass epoxy board and a 25 μm thick copper foil) was etched to open dents (openings) with a diameter of 100 μm and a depth of 25 μm in a straight line across a 30 mm square area in the center of the board, with the distance between the centers of adjacent holes being 900 μm. In this way, an evaluation board with a total of 900 dents was prepared.
[0244] The resin film side of the obtained laminated film was placed on the evaluation substrate, and heated and pressed at a lamination pressure of 0.4 MPa for 20 seconds, a press pressure of 0.8 MPa for 20 seconds, and a lamination and press temperature of 90°C using a Meiki Seisakusho "Batch Type Vacuum Laminator MVLP-500-IIA." After cooling to room temperature, the PET film was peeled off. In this way, an evaluation sample in which a resin film was laminated on an evaluation substrate was obtained.
[0245] The obtained evaluation samples were observed for voids in the recesses using an optical microscope. The ratio of recesses in which voids were observed was evaluated to determine the embeddability of the sample against the uneven surface according to the following criteria.
[0246] [Criteria for embeddability on uneven surfaces] ○: The percentage of depressions where voids were observed was 0%. △: The percentage of depressions where voids were observed was more than 0% and less than 5%. ×: The percentage of depressions in which voids were observed was 5% or more.
[0247] The obtained evaluation samples were observed using an optical microscope to see whether or not the resin film protruded from a predetermined area on the substrate, and the protrusion prevention property was judged according to the following criteria.
[0248] [Criteria for determining anti-extrusion performance] ○: The resin film protrudes less than 2 mm from the periphery of the evaluation board after lamination. △: After lamination, the resin film protrudes from the periphery of the evaluation board by more than 2 mm and 3 mm or less. ×: The resin film protrudes from the periphery of the evaluation board after lamination by more than 3 mm.
[0249] (3) Undulation A mask was attached to the 18 μm thick copper layer so that a rectangular area of 1 mm length x 2 mm width was etched, and the copper was etched to prepare a 100 mm square substrate having a rectangular depression of 1 mm x 2 mm. Both sides of the copper foil surface of this substrate were immersed in "Cz8101" manufactured by Mec Co., Ltd. to roughen the copper foil surface. Using "Batch Vacuum Laminator MVLP-500-IIA" manufactured by Meiki Seisakusho Co., Ltd., the resin film (B stage film) side of the laminate film was laminated on both sides of the roughened substrate to obtain a laminated structure. The lamination conditions were as follows: decompression for 30 seconds to make the air pressure 13 hPa or less, then lamination at 100 ° C and pressure 0.7 MPa for 30 seconds, and further pressing at a press pressure of 0.8 MPa and a press temperature of 100 ° C for 60 seconds. The PET film was peeled off, and the resin film was heated at 100°C for 30 minutes, and then further heated at 180°C for 30 minutes to semi-cure the resin film. The surface of the semi-cured resin film where the copper pattern was present (the surface opposite the substrate) and the surface of the semi-cured resin film where the copper pattern was not present (the surface opposite the substrate) were observed, and the maximum difference in height between adjacent concave and convex portions was measured using an optical step gauge and used as the undulation value.
[0250] [Undulation criteria] ○: Undulation value is 2μm or less ×: Undulation value exceeds 2 μm
[0251] The compositions and results are shown in Table 1 below.
[0252] [Table 1] [Explanation of symbols]
[0253] 11...Multilayer printed wiring board 12...Circuit board 12a…Top surface 13~16…Insulating layer 17...Metal layer
Claims
1. A composition comprising a maleimide compound, a curing accelerator, a thermoplastic resin, optionally an inorganic filler, and optionally a solvent; The weight average molecular weight of the thermoplastic resin is 20,000 or more, the maleimide compound has a skeleton derived from a dimer diamine, a skeleton derived from pyromellitic dianhydride, and a skeleton derived from an aliphatic diamine compound, the aliphatic diamine compound has a ring structure including a cyclohexane skeleton, when a maleimide compound-containing liquid containing 5% by weight of the maleimide compound and 95% by weight of cyclohexanone is obtained, the maleimide compound exhibits a property that the maleimide compound-containing liquid has a haze of 5% or more, A resin material in which the content of the maleimide compound is 5% by weight or more based on 100% by weight of components excluding inorganic fillers and solvents in the resin material.
2. The resin material according to claim 1 , wherein the maleimide compound has a weight average molecular weight of 1,000 or more and 50,000 or less.
3. The resin material according to claim 1 or 2, wherein the maleimide compound has a structure represented by the following formula (X): [Formula 1] In the formula (X), R1 represents a tetravalent organic group.
4. The resin material according to any one of claims 1 to 3, wherein the curing accelerator includes a photocuring accelerator.
5. The present invention comprises a curable compound different from the maleimide compound, The resin material according to any one of claims 1 to 4, wherein the curable compound includes a curable compound having a weight average molecular weight of less than 1,500.
6. A thermosetting compound different from the maleimide compound and a curing agent, The resin material according to any one of claims 1 to 5, wherein the thermosetting compound includes an epoxy compound.
7. The resin material according to claim 6 , wherein the hardener comprises an active ester compound.
8. The resin material according to any one of claims 1 to 7, further comprising an inorganic filler.
9. The resin material according to claim 8 , wherein the content of the inorganic filler is 50% by weight or more based on 100% by weight of components excluding the solvent in the resin material.
10. The resin material according to claim 8 or 9, wherein the inorganic filler is silica.
11. The resin material according to any one of claims 1 to 10, which is a resin film.
12. The resin material according to any one of claims 1 to 11, which is used to form an insulating layer in a multilayer printed wiring board.
13. A circuit board; a plurality of insulating layers disposed on a surface of the circuit board; a metal layer disposed between a plurality of the insulating layers; A multilayer printed wiring board, wherein at least one of the insulating layers is a cured product of the resin material according to any one of claims 1 to 12.
Citation Information
Patent Citations
Resin for optical-semiconductor-element encapsulation containing polyimide and optical semiconductor device obtained with the same
JP2009114415A
Epoxy resin composition
JP2013234328A
Resin composition for electronic material
JP2018090728A
Resin composition
JP2019044128A
Resin composition, support with resin layer, prepreg, laminate, multilayered printed wiring board, and printed wiring board for millimeter-wave radar
WO2016114286A1