Manufacturing method for precast remaining formwork panels

The use of volcanic lapilli and ash aggregates with a chemical reaction to form a waterproof layer in precast panels addresses capillary void issues, preventing moisture ingress and cracking, while reducing panel weight and improving durability.

JP7596586B1Active Publication Date: 2024-12-09山下譲二

Patent Information

Application Number
JP2024087667
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2024-05-30
Publication Date
2024-12-09
Estimated Expiration
2044-05-30

AI Technical Summary

Technical Problem

Conventional methods for manufacturing precast residual formwork panels fail to completely close capillary voids, leading to moisture ingress and potential alkali-silica reactions that cause cracking over time, and there is a need for lightweight panels to reduce manual labor in transportation.

Method used

The method involves using volcanic lapilli and volcanic ash as aggregates, mixing with heated water to create a fluidized cement composition, molding with excess water pushed to the back surface, and allowing a chemical reaction to form a waterproof layer that blocks capillary voids, using stainless steel fittings if necessary, to prevent moisture ingress and alkali-silica reactions.

Benefits of technology

The method results in lightweight panels that prevent cracking due to alkali-silica reactions by nearly completely closing capillary voids, improving water impermeability and reducing panel weight by 30-40% compared to conventional methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007596586000001_ABST
    Figure 0007596586000001_ABST
Patent Text Reader

Abstract

To provide a manufacturing method for a precast remaining form panel, which can manufacture a lightweight precast remaining form panel, improve the water impermeability of the precast concrete panel body, and prevent cracks caused by aging. [Solution] A manufacturing method for precast remaining form panels is a manufacturing method for precast remaining form panels that manufactures non-permeable precast remaining form panels using volcanic lapilli and volcanic ash as lightweight aggregates, and includes a mixing process of mixing concrete raw materials containing cement, volcanic lapilli as coarse aggregate and volcanic ash as fine aggregate with mixing water to obtain a fluidized cement composition, and an insulation curing process of allowing the temperature of the fluidized cement composition poured into the forming formwork to naturally drop to the outside air temperature without reheating the fluidized cement composition from the outside, thereby preventing the bleeding phenomenon in which the fluidized cement composition is discharged outside the forming formwork.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for manufacturing a precast remaining form panel that can suppress cracks due to alkali-aggregate reaction. [Background technology]

[0002] Precast remaining form panels are made of concrete. Conventionally, cracks that occur when making precast remaining form panels and cracks that occur due to deterioration of concrete after constructing a wall (remaining form) made of precast remaining form panels have been problems. Alkali-aggregate reaction is known as a concrete deterioration phenomenon. In alkali-aggregate reaction, an alkaline aqueous solution contained in concrete reacts with aggregates such as gravel and sand, causing expansion and cracks due to expansion. Alkali-silica reaction is known as one of the alkali-aggregate reactions. In this alkali-silica reaction, silica minerals in aggregate react with alkaline components in concrete to produce silica gel, which absorbs water and expands inside the concrete, and the pressure of the expansion causes cracks from the inside. There are tortoiseshell-shaped cracks that occur on the surface due to the expansion of concrete, and cracks that occur perpendicular to or parallel to the reinforcing bars or horizontally.

[0003] When cracks occur in the precast remaining form panels, the remaining form, which is made up of the precast remaining form panels, may suffer from frost damage, salt damage, efflorescence, etc. In order to prevent such cracks, frost damage, salt damage, efflorescence, etc., the inventor has proposed a manufacturing method for a precast remaining form panel for sealing voids formed in the precast remaining form panels, such as capillary voids (for example, Patent Document 1).

[0004] The manufacturing method of the precast remaining form panel described in Patent Document 1 includes a step of pouring a fluidized cement composition obtained by mixing concrete raw materials including cement, gravel, and sand, 5% to 40% by weight of limestone fine powder relative to the cement in the concrete raw materials, and mixing water, or a fluidized cement composition obtained by mixing mortar raw materials including cement and sand, 5% to 40% by weight of limestone fine powder relative to the cement in the mortar raw materials, and mixing water, into a molding form, a molding step of molding the fluidized cement composition poured into the molding form, and a curing step of hardening the fluidized cement composition. In this manufacturing method of the precast remaining form panel, in the molding step and the curing step, excess water containing calcium hydroxide dissolved from the cement is pushed up to the back side in the mixing water, so that it is stored in the entire back area of ​​the panel body, covering the back side of the panel body with the excess water, and the excess water is present so as to fill capillary voids formed inside the panel body. When the cement in the fluidized cement composition hardens, a waterproof layer is formed over the entire back surface of the panel body, which prevents the carbon dioxide in the outside air from chemically reacting with calcium hydroxide and forming a permeable fine powder layer of calcium carbonate over the entire back surface of the panel body, and at the same time, capillary voids, etc. are naturally blocked by the waterproof layer. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent No. 7314430 Summary of the Invention [Problem to be solved by the invention]

[0006] Conventional manufacturing methods have been effective in blocking capillary voids, but they do not completely block capillary voids. This means that moisture can penetrate into the precast remaining formwork panel through the formed capillary voids, and react with silica minerals, causing an alkali-silica reaction. In addition, moisture continues to penetrate, accelerating the alkali-silica reaction and causing cracks several years later. In light of this, there has been a demand for a manufacturing method for precast remaining formwork panels that can completely block capillary voids in precast concrete panels, prevent moisture from penetrating, and suppress expansion cracks caused by alkali-silica reactions.

[0007] Furthermore, in recent years, there has been a demand for lightweight precast remaining form panels, as crack formation is suppressed and the transportation of precast remaining form panels is done manually. Specifically, there is a demand to reduce the weight from the current 21 kg to around 16 kg.

[0008] Therefore, an object of the present invention is to provide a method for manufacturing a precast remaining form panel that can produce a lightweight precast remaining form panel and can suppress cracking over time due to alkali-aggregate reaction. [Means for solving the problem]

[0009] The method for producing a precast remaining form panel according to the present invention is a method for producing a non-permeable precast remaining form panel using volcanic lapilli and volcanic ash as aggregates, and includes a mixing step of mixing concrete raw materials containing cement, the volcanic lapilli as coarse aggregate, and the volcanic ash as fine aggregate with mixing water for hydration reaction that has been heated to a temperature of 60°C to 85°C in advance, to obtain a fluidized cement composition with a mixing temperature of 15°C to 45°C corresponding to an outside air temperature of 0°C to 40°C, and a mixing step of mixing the panel body so that the rear surface of the panel body faces upward and the fluidized cement composition is poured into a molding form designed to be kept horizontal and in a vertical position; excess water containing calcium hydroxide dissolved from the cement in the mixing water is pushed up toward the rear surface of the panel body, so that the excess water is stored over the entire rear surface of the panel body and covers the rear surface of the panel body; and the excess water is allowed to fill capillary voids formed inside the panel body. In this manner, vibration is applied to the fluidized cement composition poured into the molding form, thereby molding the fluidized cement composition poured into the molding form. After the step of molding the fluidized cement composition, the temperature of the fluidized cement composition in the molding frame is naturally lowered to an outside temperature over a period of 3 hours or more without externally reheating the fluidized cement composition charged into the molding frame, thereby suppressing a bleeding phenomenon in which mixing water for hydration reaction containing calcium hydroxide dissolved from the fluidized cement composition expands in volume and is discharged to the outside of the molding frame, thereby suppressing the generation of capillary voids in the fluidized cement composition and maintaining the fluidized cement composition in a state where a demolding strength is ensured. and a demolding process of removing the molding form after the thermal curing process, in which, when the fluidized cement composition hardens in the thermal curing process, an alkaline component contained in the fluidized cement composition reacts chemically with silica contained in the volcanic gravel and volcanic ash to generate alkaline silica gel, thereby forming a waterproof layer over the entire back surface of the panel body, and preventing carbon dioxide in the outside air from chemically reacting with the calcium hydroxide to form a water-permeable fine powder layer of calcium carbonate over the entire back surface of the panel body, while at the same time preventingThe capillary voids are almost completely blocked by the waterproof layer, dramatically improving the water impermeability of the panel body, and preventing expansion cracks caused by alkali-silica reaction of the coarse aggregate of the volcanic lapilli and the fine aggregate of the volcanic ash over time.

[0010] The manufacturing method of the precast remaining formwork panel of the present invention is characterized in that in the step of molding the fluidized cement composition, a stainless steel connecting fitting is embedded in the back surface of the panel body. Effect of the Invention

[0011] In the method for manufacturing a precast remaining form panel according to the present embodiment, concrete raw materials including cement, volcanic lapilli as a coarse aggregate, and volcanic ash as a fine aggregate are used. Since volcanic lapilli and volcanic ash are lightweight aggregates, the manufactured precast remaining form panel is lighter than conventional panels.

[0012] The method for manufacturing a precast remaining form panel according to the present invention involves mixing concrete raw materials containing cement, volcanic lapilli coarse aggregate, and volcanic ash fine aggregate with mixing water for hydration reaction that has been heated to a temperature of 60°C to 85°C in advance, to obtain a fluidized cement composition with a mixing temperature of 15°C to 45°C corresponding to an outside air temperature of 0°C to 40°C, and allowing the temperature of the fluidized cement composition in the forming form to drop naturally to the outside air temperature over a period of 3 hours or more without reheating the fluidized cement composition from the outside. This prevents the bleeding phenomenon, in which the mixing water for hydration reaction containing calcium hydroxide eluted from the fluidized cement composition expands in volume and is discharged outside the forming form, thereby preventing the generation of capillary voids in the fluidized cement composition, and moisture does not penetrate into the inside of the panel body, so that an alkali-silica reaction does not occur in the coarse aggregate of volcanic lapilli and the fine aggregate of volcanic ash, and prevents expansion cracks caused by the alkali-silica reaction. Therefore, the precast remaining formwork panel is prevented from undergoing expansion cracking over time.

[0013] In addition, in the manufacturing method of the precast remaining form panel using the concrete raw material, in the heat retention curing step, excess water containing calcium hydroxide dissolved from the cement in the mixing water is pushed up to the back side, and is stored on the entire back side of the panel body, covering the back side of the panel body with the excess water, and the excess water is present so as to fill voids such as capillary voids formed inside the panel body, and when the fluidized cement composition hardens, the alkaline component contained in the fluidized cement composition reacts chemically with the silica contained in the volcanic lapilli and volcanic ash to generate alkaline silica gel, forming a waterproof layer on the entire back side of the panel body, which can prevent the formation of a permeable calcium carbonate fine powder layer on the entire back side of the panel body. The waterproof layer almost completely blocks voids such as capillary voids, dramatically improving the impermeability of the panel body.

[0014] In the method for manufacturing a precast remaining form panel according to the present invention, the stainless steel connecting fittings can be embedded in a predetermined position in the fluidized cement composition so that they protrude from the back surface of the panel body in the inserting step. Even in this case, the gap formed between the embedded part of the connecting fittings and the panel body is almost completely filled with the waterproof layer, dramatically improving the water impermeability of the panel body. [Brief description of the drawings]

[0015] [Figure 1] 1A and 1B are diagrams illustrating a precast remaining form panel according to an embodiment of the present invention, in which (a) is a cross-sectional view and (b) is a rear view. [Diagram 2] FIG. 2 is an enlarged view of a connected portion of a precast remaining formwork panel according to an embodiment of the present invention. [Diagram 3] 1A, 1B, and 1C are diagrams for explaining a manufacturing process of a precast remaining form panel according to an embodiment of the present invention. [Figure 4] 1A and 1B are diagrams showing a remaining formwork constructed by a remaining formwork construction method according to an embodiment of the present invention, in which (a) shows a cross-sectional view and (b) shows a front view. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] The manufacturing method of a precast remaining form panel according to the present invention will be described with reference to Fig. 1 to Fig. 4. In the drawings, the horizontal direction of the precast remaining form panel is indicated as width direction X, the vertical direction is indicated as height direction Y, and the thickness direction is indicated as front-rear direction Z.

[0017] In the manufacturing method of a precast remaining form panel according to this embodiment, a non-water-permeable precast remaining form panel 1 shown in Fig. 1 is manufactured. As shown in Fig. 1(a), this precast remaining form panel 1 comprises a precast remaining form panel body 2 (hereinafter also referred to as the panel body 2), a plurality of connected metal fittings 3 provided at predetermined positions on the back surface 2a of the panel body 2, and a waterproof layer 4 formed on the back surface 2a etc. of the panel body 2. This precast remaining form panel 1 is a non-water-permeable precast remaining form panel that uses volcanic lapilli and volcanic ash as lightweight aggregate.

[0018] [Panel body 2] 1(a) and 1(b), the panel body 2 is rectangular, and a panel body 2 having a height of 300 mm and a width of 900 mm is used, for example. Two connected metal fittings 3 are provided in the width direction X and the height direction Y on the back surface 2a of the panel body 2. The connected metal fittings 3 are provided so as to protrude from the back surface 2a of the panel body 2. A plurality of reinforcing bars 5 are provided inside the panel body 2 in the width direction X and the height direction Y to ensure the strength of the panel body 2. The size (height and width) of the panel body 2 can be changed as appropriate.

[0019] [Connected metal fitting 3] The connected metal fitting 3 comprises a hook portion 6 and an embedded portion 7 connected to both ends of the hook portion 6 (Fig. 1(a)). The connected metal fitting 3 is attached to the panel main body 2 with the embedded portion 7 embedded inside the panel main body 2 and the hook portion 6 protruding from the back surface 2a of the panel main body 2. The connected metal fitting 3 can be made of metal, and is preferably made of a material with excellent corrosion resistance, such as stainless steel (SUS304).

[0020] [Waterproof layer 4] The waterproof layer 4 is formed by a chemical reaction between the alkaline component contained in the fluidized cement composition C and the silica contained in the volcanic lapilli and volcanic ash to produce alkaline silica gel, which is insoluble in water. Layer As shown in FIG. 2, the waterproof layer 4 is formed over the entire back surface 2a of the panel body 2, as well as in the capillary gap 9A and the gap 9B formed between the embedded portion 7 of the connected metal fitting 3 and the panel body 2.

[0021] Next, a method for manufacturing a precast remaining form panel will be described.

[0022] The manufacturing method of the precast remaining form panel according to the present embodiment is a method for manufacturing a non-permeable precast remaining form panel 1. The manufacturing method of the precast remaining form panel includes a mixing step of mixing concrete raw materials including cement, volcanic gravel as coarse aggregate and volcanic ash as fine aggregate with mixing water for hydration reaction heated to a predetermined temperature in advance to obtain a fluidized cement composition C having a predetermined mixing temperature corresponding to an outside air temperature of 0°C to 40°C, a charging step of charging the fluidized cement composition C into a molding form 22 after the mixing step, a molding step of molding the fluidized cement composition C charged into the molding form 22, a heat retention curing step of naturally lowering the temperature of the charged fluidized cement composition C to the outside air temperature over a predetermined time or more without reheating the charged fluidized cement composition C from the outside, and hardening the fluidized cement composition C, and a demolding step of removing the molding form 22 after the heat retention curing step. In the method for producing a recast remaining form panel according to the present invention, no heating is carried out in the mixing step except for heating the mixing water for the hydration reaction to increase its temperature.

[0023] [Mixing process] In the mixing step, concrete raw materials including cement, volcanic gravel as coarse aggregate, and volcanic ash as fine aggregate are mixed with mixing water for hydration reaction that has been heated to a temperature of 60°C to 85°C in advance, to obtain a fluidized cement composition with a mixing temperature of 15°C to 45°C corresponding to an outside air temperature of 0°C to 40°C. Note that the mixing temperature is preferably 15°C higher than 0°C when the outside air temperature is 0°C in winter, and is preferably 5°C higher than 40°C when the outside air temperature is 40°C in summer.

[0024] [Feeding process] In the pouring step, as shown in FIG. 3, the panel body 2 is formed using a molding formwork 22. The molding formwork 22 is designed so that the back surface 2a of the panel body 2 faces upward and is maintained horizontally. The upper side of the molding formwork 22 becomes the back surface 2a side of the panel body 2. Specifically, as shown in FIG. 3(a), a mixture with the fluidized cement composition C is poured into the molding formwork 22 installed on a stand 21 equipped with a vibration device 20, and the fluidized cement composition C is vibrated by the vibration device 20. Then, excess water containing calcium hydroxide eluted from the fluidized cement composition C is pushed up to the back surface 2a side of the panel body 2. Then, this excess water is interposed so as to fill the capillary gap 9A formed inside the panel body 2 and the gap 9B formed between the embedded part 7 of the connected metal fitting 3 and the panel body 2, and the entire back surface of the panel body 2 is covered with excess water containing calcium hydroxide.

[0025] [Burial process] After the pouring step, as shown in Figures 3(b) and (c), the connected metal fittings 3 attached to the reinforcing bars 5 are embedded in the fluidized cement composition C poured into the forming formwork 22. Specifically, the connecting portion of the hook portion 6 and the embedded portion 7 and the embedded portion 7 are pushed into the fluidized cement composition C to a predetermined position, and the hook portion 6 of the connected metal fittings 3 are embedded so as to protrude from the back surface 2a of the panel main body 2. Note that if the connected metal fittings 3 are not formed integrally with the panel main body 2, the embedding step is not performed.

[0026] [Thermal curing process] In the heat-retaining curing step, the fluidized cement composition C is hardened until the demolding strength is ensured. Specifically, the fluidized cement composition C, which has been poured into the molding frame 22 and is at a temperature higher than the outside air temperature, is allowed to naturally drop in temperature to the outside air temperature over a period of 3 hours or more without being reheated from the outside. When the temperature is naturally lowered to the outside air temperature, the mixing water for the hydration reaction, which contains calcium hydroxide dissolved from the fluidized cement composition C, expands in volume and is discharged to the outside of the molding frame 22, thereby preventing the bleeding phenomenon. By preventing bleeding, the generation of capillary voids 9A and voids 9B in the fluidized cement composition C is prevented.

[0027] In the heat-retaining curing process, excess water containing calcium hydroxide dissolved from the cement is pushed up to the rear surface 2a side in the mixing water, and is stored in the entire rear surface 2a of the panel body 2. The excess water covers the rear surface 2a of the panel body 2, and the excess water is present so as to fill the capillary voids 9A and voids 9B formed inside the panel body 2. When the fluidized cement composition C hardens, the alkaline component contained in the fluidized cement composition C reacts chemically with the silica contained in the volcanic lapilli and volcanic ash to generate alkaline silica gel, forming a waterproof layer 4 over the entire rear surface 2a of the panel body 2. This prevents the formation of a permeable calcium carbonate fine powder layer over the entire rear surface 2a of the panel body 2. Furthermore, the waterproof layer 4 almost completely blocks the capillary voids and voids 9B.

[0028] [Demolding process] In the demolding process, the molding frame 22 is removed after a heat-retaining curing process is performed for a predetermined time.

[0029] Next, a construction method using the precast remaining form panel 1 manufactured by the above-mentioned manufacturing method will be described. The cement-based binder used in the remaining form construction method can be anything that contains moisture and hardens over time, such as concrete, mortar, and aerated mortar. In this embodiment, an example will be described in which ready-mixed concrete 12 is used as the cement-based binder.

[0030] In the construction method according to this embodiment, as shown in Fig. 4(b), precast remaining form panels 1 are stacked to construct a remaining form 10. In this precast remaining form panel 1, a waterproof layer 4 is formed in the entire back surface 2a of the panel body 2, in the capillary gaps 9A, and in the gaps 9B. When constructing the remaining form 10, as shown in Fig. 4(a), the precast remaining form panel 1 is fixed to the front surface of the wooden form 13 by connecting the precast remaining form panel 1 to the wooden form (concrete panel) 13 using steel connecting fittings (separators) 11 connected to the connected fittings 3.

[0031] Next, a cement-based solidifying material casting process is performed. Specifically, fresh concrete 12 is cast between the remaining precast formwork panel 1 and the wooden formwork 13 (FIG. 4(a)). The fresh concrete 12 is cast so as to come into contact with the waterproof layer 4 formed on the back surface 2a of the panel body 2.

[0032] After pouring the ready-mixed concrete 12, the ready-mixed concrete 12 is hardened (cement-based binder hardening step). At this time, since the waterproof layer 4 is formed in the capillary voids 9A and the voids 9B, the moisture in the ready-mixed concrete 12 is prevented from penetrating into the inside of the panel body 2 through the capillary voids 9A and the voids 9B. This prevents the moisture in the ready-mixed concrete 12 from being released and evaporated, and prevents cracks in the ready-mixed concrete 12 due to drying shrinkage.

[0033] Next, the effects of the method for manufacturing a precast remaining form panel according to this embodiment will be described.

[0034] In the manufacturing method of the precast remaining form panel according to the present embodiment, concrete raw materials including cement, volcanic lapilli as coarse aggregate, and volcanic ash as fine aggregate are used. Since volcanic lapilli and volcanic ash are lightweight aggregates, the manufactured precast remaining form panel is lighter than conventional panels. Specifically, the weight of the precast remaining form panel manufactured by the manufacturing method of the precast remaining form panel according to the present embodiment is 30% to 40% less than that of the conventional panel using gravel or sand.

[0035] The precast remaining formwork panel 1 according to this embodiment is prepared by mixing concrete raw materials containing volcanic lapilli as coarse aggregate and volcanic ash as fine aggregate with mixing water for hydration reaction that has been heated in advance to obtain a fluidized cement composition with a mixing temperature of 15°C to 45°C corresponding to an outside air temperature of 0°C to 40°C, and then allowing the temperature to rise naturally to the outside air temperature without heating. This causes the alkaline component contained in the fluidized cement composition C to react chemically with the silica contained in the volcanic lapilli and volcanic ash to produce alkaline silica gel, forming a waterproof layer 4 over the entire back surface 2a of the panel main body 2, and filling the capillary voids 9A and the voids 9B (not shown in the drawing) formed between the embedded parts 7 of the connected metal fittings 3 and the panel main body 2 with water-insoluble substances. Defense It is almost completely blocked by the water layer 4. In this way, by forming the waterproof layer 4, it is possible to prevent the formation of a water-permeable fine powder layer of calcium carbonate over the entire back surface 2a of the panel body 2, and it almost completely blocks the capillary gap 9A and the gap 9B formed between the embedded portion 7 of the connected metal fitting 3 and the panel body 2. This prevents moisture from penetrating into the inside of the panel body 2, prevents alkali-silica reaction of the coarse aggregate of the volcanic lapilli and the fine aggregate of the volcanic ash, inhibits expansion cracks caused by the alkali-silica reaction, and inhibits expansion cracks that occur over time.

[0036] Furthermore, by forming the waterproof layer 4, it is possible to prevent the formation of a water-permeable fine powder layer of calcium carbonate over the entire back surface 2a of the panel body 2, and by almost completely blocking the capillary gap 9A and the gap 9B formed between the embedded portion 7 of the connected metal fitting 3 and the panel body 2, it is possible to dramatically improve the water impermeability of the panel body 2. Since the water impermeability of the panel body 2 is dramatically improved, this is particularly suitable for a panel body 2 having a thin thickness.

[0037] In the manufacturing method of the precast remaining form panel according to this embodiment, concrete raw materials containing volcanic gravel as a coarse aggregate and volcanic ash as a fine aggregate are used, and therefore the hydration reaction is significantly faster than when fine silica powder is used, for example, and therefore the waterproof layer 4 can be formed in a short time on the back surface 2a of the panel main body 2 and on the capillary voids 9A and voids 9B. In addition, the hydration reaction is not slowed down even at low temperatures (for example, 5 degrees), so the manufacturing method according to this embodiment is particularly useful when manufacturing the panel main body 2 at low temperatures.

[0038] Furthermore, the manufacturing method of the precast remaining form panel according to this embodiment contributes to energy saving because the temperature of the fluidized cement composition C is naturally lowered to the outside air temperature over a period of 3 hours or more in the thermal curing step without reheating the fluidized cement composition C from the outside. The construction method using the precast remaining form panel 1 according to this embodiment allows the appearance of the remaining form 10 to be maintained after construction, and the remaining form 10 to be stably maintained for a long period of time without reducing durability.

[0039] In addition, in the precast remaining form panel 1 used in this embodiment, the waterproof layer 4 is formed, and the capillary voids 9A and voids 9B of the panel body 2 are almost completely blocked, so that the water in the poured fresh concrete 12 is prevented from being rapidly released and evaporated from the capillary voids 9A during the cement-based hardening material hardening process. Therefore, the fresh concrete 12 gradually hardens and is less likely to crack, and cracks are prevented from occurring in the panel body 2 after the remaining formwork 10 is constructed. In this way, the effect of the fresh concrete 12 gradually hardening and thus making it less likely to crack is effective when constructing the remaining formwork 10 in the summer or when constructing the remaining formwork 10 in a sunny location.

[0040] As described above, by using the construction method of this embodiment, deterioration of the precast remaining formwork panel 1 due to salt damage or frost damage can be prevented, cracks can be prevented from occurring in the precast remaining formwork, and the surface of the remaining formwork can be prevented from becoming contaminated.

[0041] Although the present embodiment has been described above, it is possible to select from the configurations given in the above embodiment, or to change to other configurations as appropriate, without departing from the spirit of the present invention.

[0042] In this embodiment, in the manufacturing method of the precast remaining form panel, the aggregate used in the raw concrete material can be only volcanic lapilli and volcanic ash. In this embodiment, the example in which the connected metal fittings 3 are embedded so as to protrude from the back surface 2a of the panel body 2 and are formed integrally therewith has been described, but the connected metal fittings can also be attached after the panel body is formed. For example, screw holes are formed in each of the four corners of the back surface of the panel body, and the connected metal fittings are fixed to these screw holes. [Explanation of symbols]

[0043] 1 Precast remaining formwork panels (panels) 2 Precast remaining formwork panel body (panel body) 2a Back (back side) 3 Connecting metal fittings 4 waterproof layer 5. Reinforcement 6 Hook part 7 Buried section 9A Capillary void 9B gap (gap formed between embedded portion 7 and panel body 2) 10 Remaining formwork 11 Connecting fittings (separators) 12 Ready-mix concrete (cement-based binder) 13 Wooden formwork (plywood) 20 Vibration device 21 units 22 Forming mold C. Fluidized cement composition X Width direction Y Height direction Z front and back direction

Claims

1. A method for manufacturing a precast remaining form panel using only volcanic gravel and volcanic ash as aggregate, comprising the steps of: A mixing process of mixing concrete raw materials including cement, the volcanic gravel as a coarse aggregate, and the volcanic ash as a fine aggregate with mixing water for hydration reaction that has been heated to a temperature of 60°C to 85°C in advance, to obtain a fluidized cement composition having a mixing temperature of 15°C to 45°C, which is higher than the outside air temperature; a step of pouring the fluidized cement composition into a molding form designed so that the rear surface of the panel body faces upward and is maintained horizontally after the mixing step, and vibrating the fluidized cement composition poured into the molding form, so that excess water containing calcium hydroxide dissolved from the cement in the mixing water is pushed up toward the rear surface of the panel body, thereby being stored over the entire rear surface of the panel body, covering the rear surface of the panel body with the excess water, and filling capillary voids formed inside the panel body, thereby molding the fluidized cement composition poured into the molding form; a heat retention curing step of naturally lowering the temperature of the fluidized cement composition in the molding form to an outside temperature over a period of 3 hours or more without externally reheating the fluidized cement composition charged into the molding form, thereby preventing the occurrence of capillary voids in the fluidized cement composition and hardening the fluidized cement composition until a demolding strength is ensured, while preventing the volume expansion of the mixing water for hydration reaction containing calcium hydroxide dissolved from the fluidized cement composition and causing a bleeding phenomenon in which the mixing water is discharged to the outside of the molding form. A demolding process of removing the molding form after the heat retention and curing process, When the fluidized cement composition hardens in the heat retention curing process, the alkaline component contained in the fluidized cement composition reacts chemically with the silica contained in the volcanic lapilli and volcanic ash to generate alkaline silica gel, forming a waterproof layer over the entire back surface of the panel body, which prevents the carbon dioxide in the outside air from reacting chemically with the calcium hydroxide to form a permeable fine powder layer of calcium carbonate over the entire back surface of the panel body, and at the same time, the capillary voids are almost completely blocked by the waterproof layer, dramatically improving the impermeability of the back surface of the panel body and suppressing expansion cracks caused by the alkali-silica reaction of the coarse aggregate of the volcanic lapilli and the fine aggregate of the volcanic ash over time. A method for manufacturing a precast remaining form panel, comprising:

2. In the step of molding the fluidized cement composition, a stainless steel connecting fitting is embedded in the back surface of the panel body. The method for manufacturing a precast remaining form panel according to claim 1 .

Citation Information

Patent Citations

  • Vertical manufacture method for scoria concrete sandwich thermal insulation external wall panel

    CN106926359A

  • Braun tube indicator

    JP1978013457A

  • Concrete form panel

    JP1996035326A

  • Manufacturing method for precast remaining formwork panels

    JP7314430B1

  • JPP6537754B

Cited By

  • Method for manufacturing precast concrete products and precast mortar products using crushed andesite aggregate