Resin particles, resin particles for toner, toner, method for manufacturing resin particles, method for manufacturing toner, developer, toner storage unit, and image forming apparatus
Resin particles with a specific crystalline resin content and 14C concentration improve carbon neutrality and performance in toners by enhancing low-temperature fixability and filming resistance, overcoming the challenges of using renewable resources in toner materials.
Patent Information
- Application Number
- JP2022164274
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-02-18
- Filing Date
- 2022-10-12
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2042-10-12
AI Technical Summary
Existing toner materials, particularly binder resins, contribute to global warming due to their reliance on fossil fuels, and transitioning to renewable resources like polylactic acid and rosin compounds faces challenges in achieving both low-temperature fixability and filming resistance.
Resin particles composed of an amorphous polyester resin and a crystalline resin, with a crystalline resin content within 150 nm of the surface limited to 4% and a 14C concentration of 5.4 pMC or higher, utilizing propylene glycol as the alcohol monomer, enhance carbon neutrality and provide excellent low-temperature fixability and filming resistance.
The resin particles significantly contribute to carbon neutrality while maintaining excellent low-temperature fixability and filming resistance, addressing the limitations of renewable resource toners.
Smart Images

Figure 0007947888000016 
Figure 0007947888000017 
Figure 0007947888000018
Abstract
Description
[Technical Field]
[0001] The present invention relates to resin particles, resin particles for toner, toner, a method for manufacturing resin particles, a method for manufacturing toner, a developer, a toner storage unit, and an image forming apparatus. [Background technology]
[0002] Traditionally, the constituent materials of toner, particularly the binder resins, have relied almost entirely on fossil fuels. When toner and printed images are discarded, the resulting carbon dioxide is released into the atmosphere, contributing to global warming. Furthermore, the shift from finite fossil fuels to renewable biomass resources is a desirable technology, as biomass resources are sustainably renewable resources, given that living organisms are produced from solar energy, water, and carbon dioxide. Therefore, the use of resins made from renewable resources such as polylactic acid (PLA) and rosin compounds as binder resins for toner is being considered.
[0003] On the other hand, in order to function as a toner, it needs basic properties such as low-temperature fixability and filming resistance. For example, a toner with excellent low-temperature fixability has been proposed that contains a polyester using propylene glycol derived from plants, which is a renewable resource, as a monomer (see Patent Document 1). [Overview of the Initiative] [Problems that the invention aims to solve]
[0004] The present invention aims to provide resin particles that make a significant contribution to carbon neutrality and exhibit excellent low-temperature fixation and filming resistance. [Means for solving the problem]
[0005] The resin particles of the present invention as a means for solving the above problem are resin particles containing at least a binder resin, wherein the binder resin is composed of an amorphous polyester resin and a crystalline resin, the alcohol monomer of the amorphous polyester resin contains propylene glycol, and the proportion of the crystalline resin present in a region within 150 nm from the outermost surface of the resin particles is 4% or less relative to the total amount of the resin particles, and the radioactive carbon isotope 14 C concentration is 5.4 pMC or higher.
Effects of the Invention
[0006] According to the present invention, it is possible to provide resin particles that greatly contribute to carbon neutrality and are excellent in low-temperature fixability and filming resistance.
Brief Description of the Drawings
[0007] [Figure 1] Figure 1 is a schematic diagram for explaining the crystalline resin inside the resin particles of the present invention. [Figure 2] Figure 2 is a schematic configuration diagram showing an example of the image forming apparatus of the present invention. [Figure 3] Figure 3 is a schematic configuration diagram showing another example of the image forming apparatus of the present invention. [Figure 4] Figure 4 is a schematic configuration diagram showing still another example of the image forming apparatus of the present invention. [Figure 5] Figure 5 is a partially enlarged view of Figure 4. [Figure 6] Figure 6 is a schematic configuration diagram showing an example of a process cartridge as the toner storage unit of the present invention.
Mode for Carrying Out the Invention
[0008] (Resin Particles and Toner Resin) The resin particles of the present invention are resin particles containing at least a binder resin, wherein the binder resin consists of an amorphous polyester resin and a crystalline resin, the alcohol monomer of the amorphous polyester resin contains propylene glycol, the proportion of the crystalline resin in the region within 150 nm from the outermost surface of the resin particles is 4% or less of the total amount of the resin particles, and radioactive carbon isotopes 14 The C concentration is 5.4 pMC or higher.
[0009] The resin particles for toner of the present invention contain the resin particles of the present invention and, if necessary, also contain other components. The resin particles of the present invention contribute significantly to carbon neutrality and exhibit excellent low-temperature fixability and filming resistance, making them suitable for use as toner.
[0010] The resin particles and the toner resin particles may contain other components in addition to the binder resin as needed. Furthermore, from the viewpoint of carbon neutrality, it is preferable that the resin particles and the toner resin particles contain a biomass-derived resin, as described later.
[0011] The resin particles and toner resin particles according to the present invention will be described below. It should be noted that the present invention is not limited to the embodiments shown below, and can be modified within the scope of what a person skilled in the art can conceive of, including other embodiments, additions, modifications, or deletions. Any embodiment that achieves the function and effects of the present invention is included within the scope of the present invention.
[0012] <<Radiocarbon Isotopes 14 C concentration>> Radioactive carbon isotopes of the aforementioned resin particles 14 C concentration (hereinafter referred to as “ 14 The "C concentration" (sometimes referred to as "C concentration") is 5.4 pMC or higher, but preferably 20.0 pMC or higher, and more preferably 35.0 pMC or higher. 14When the C concentration is less than 5.4 pMC, it is generally easily recognized that the biomass degree described later is low, and carbon neutrality cannot be achieved.
[0013] The above-mentioned carbon neutral is generally used as a definition related to biomass substances composed of organic matter. When such a biomass substance is combusted, carbon dioxide is discharged, and the carbon contained in the carbon dioxide is derived from the carbon dioxide absorbed from the atmosphere by photosynthesis during the growth process of the biomass substance. Therefore, even if biomass substances are used, it is considered that the amount of carbon dioxide in the atmosphere does not increase as a whole. Such a property is referred to as "carbon neutrality".
[0014] The above-mentioned 14 C concentration exists in the natural world (in the atmosphere), and while plants are active, it is taken into the plants by photosynthesis, and in the carbon dioxide present in the atmosphere, the 14 C concentration and the C concentration in the carbon in the organic components of the plant are at equilibrium (107.5 pMC). However, from the stage where the plant stops its life activity, the uptake of carbon by photosynthesis stops, and the 14 C concentration decreases according to the half-life of C, which is 5,730 years. Since fossil resources derived from organisms have passed tens of thousands to hundreds of millions of years after the cessation of life activities, the above-mentioned 14 C concentration is hardly detected. 14 The above-mentioned 14 14
[0015] The above-mentioned 14 C concentration can also define how much of the carbon in the carbon element component of carbon-containing petrochemical products is plant-derived carbon. The 14 concentration of C in the carbon element of petrochemical products can be measured, for example, in accordance with ASTM-D6866, an ASTM standard of the American Society for Testing and Materials.
[0016] Here, "pMC" is an abbreviation for percent Modern Carbon, and is one of the units representing 14 C concentration. The 14C and 12 Ratio to C ( 14 C / 12 C) is defined as 100 pMC. However, the current atmospheric 14 Since the C concentration is increasing year by year, it is stipulated that this value be multiplied by a coefficient for correction. The correction coefficient to be used shall be one appropriate for that year.
[0017] The aforementioned 14 The C concentration can also be expressed as biomass percentage, calculated using the following formula (1). Biomass percentage (%) = 14 C concentration (pMC) / 107.5×100 Equation (1)
[0018] The aforementioned 14 A C concentration of 5.4 pMC or higher means that the biomass content is 5% or higher, 14 A C concentration of 20.0 pMC or higher means that the biomass content is 18.6% or higher, 14 A C concentration of 30.0 pMC or higher means that the biomass content is 27.9% or higher. A biomass content of 5% or higher is a concentration desired from the perspective of carbon neutrality.
[0019] The aforementioned 14 There are no particular restrictions on the method for measuring the C concentration, and it can be appropriately selected depending on the purpose, but radiocarbon dating is particularly preferred. The measurement procedure for the radiocarbon dating method involves burning the resin particles to reduce the CO2 (carbon dioxide) and obtain C (graphite). 14 The C concentration is measured using an accelerator mass spectrometer (AMS). This AMS measurement is disclosed, for example, in Japanese Patent No. 4050051.
[0020] <<Percentage of the crystalline resin present in the region within 150 nm from the outermost surface of the resin particles>> The resin particles have a crystalline resin content within 150 nm from the outermost surface of the resin particles that is 4% or less of the total amount of resin particles, and preferably 2% or less. Here, an embodiment of the resin particles of the present invention will be described with reference to Figure 1. Figure 1 is a schematic diagram illustrating the crystalline resin inside the resin particles of the present invention. Within the resin particle 1, there are domains 2 derived from crystalline resin and domains 3 derived from amorphous resin. In the domain 2 derived from crystalline resin, the proportion of crystalline resin is low in the region within 150 nm from the outermost surface of the resin particle 1. This indicates that the crystalline resin 2 is encapsulated within the resin particle 1. When the proportion of crystalline resin in the region within 150 nm from the outermost surface of the resin particle is 4% or less, the filming resistance is improved. Conversely, when the proportion of crystalline resin in the region within 150 nm from the outermost surface of the resin particle exceeds 4%, the desired filming resistance cannot be obtained.
[0021] In this specification, the proportion of the crystalline resin in the region within 150 nm from the outermost surface of the resin particles is a value measured by the following method. The resin particles are embedded in epoxy resin (S-31, manufactured by DEVCON), cut to a thickness of 60 nm using an ultrasonic ultramicrotome (Leica EM UC7, manufactured by Leica), and stained with ruthenium using a vacuum staining apparatus (manufactured by Philgen Co., Ltd.). Subsequently, observation is performed using a transmission electron microscope (H-7500, manufactured by Hitachi High-Tech Corporation) at an acceleration voltage of 120 kV. In this process, 50 resin particles are arbitrarily selected from those within ±2.0 μm of the weight-average particle size of the resin particles and photographed. In the configuration of the present invention, staining with ruthenium tetroxide (RuO4) projects the crystalline resin in the resin particles more intensely. If the resin particles contain wax, the wax is projected even more intensely. The proportion of crystalline resin in the region within 150 nm from the outermost surface of the resin particles can be calculated using image processing software as needed.
[0022] Image-J can be used as the image processing software. Image-J is open source, and variations in processing and additional functions can be developed as plugins by extending parts of the code. The method for calculating the proportion of crystalline resin in the region within 150 nm from the outermost surface of the resin particles using Image-J is as follows. (1) The outer periphery of all crystalline resin domains that are unevenly distributed in the cross-sectional image of a single resin particle is enclosed with freehand sections, the area is measured using Analyze, and the sum of these areas is defined as "Area A". (2) The outer circumference of one resin particle in the cross-sectional image is enclosed by freehand sections to create "region 1". (3) Determine the center of mass of "region 1" using Analyze. (4) Using a proprietary plugin, a "region 2" is created by taking 100 points at a distance of 150 nm from the center of gravity of the resin particle determined in (3) from the coordinates obtained by dividing the outer perimeter of "region 1," that is, the line that encloses the outer perimeter of one resin particle in (2) with Freehand-sections into 100 equally spaced points, and connecting these points with straight lines. (5) Create "Region 3" by subtracting "Region 2" created in (4) from "Region 1" created in (2). (6) The outer perimeter of the crystalline resin domains in "Region 3" created in (5) above is enclosed with Freehand-sections, the area is measured using Analyze, and the sum of these areas is defined as "Area B". (7) Substitute the "area A" calculated in (1) above and the "area B" calculated in (6) above into the following formula (2) to calculate the proportion of crystalline resin in the region within 150 nm from the outermost surface of one resin particle. The percentage of crystalline resin in the region within 150 nm from the outermost surface of a single resin particle [%] = Area A / Area B × 100 ... Equation (2) (8) Perform the operations described in (1) to (7) above for 50 resin particles and calculate the average value of the proportion of crystalline resin in the region within 150 nm from the outermost surface of the 50 resin particles. This average value is taken as the proportion of crystalline resin in the region within 150 nm from the outermost surface of the resin particles in this invention.
[0023] <<Biomass-derived resin>> The biomass-derived resin is a resin that contains plant-derived compounds as raw materials. The biomass-derived resin may be contained in the amorphous polyester resin, in the crystalline resin, in the coloring agent described later, or in other components such as mold release agents. In the resin particles, the toner quality when the resin particles are applied to toner can be adjusted by adjusting the ratio of petroleum-derived components to plant-derived components in the alcohol and acid components that constitute the amorphous polyester resin and the crystalline resin.
[0024] Conventionally, toners derived from renewable resources have used release agents such as carnauba wax and candelilla wax as constituent materials. These release agents are added to the toner to impart release properties during fixing, and their amount is generally around a few mass percent. Therefore, it has been difficult to satisfy carbon neutrality with release agents alone.
[0025] Therefore, in recent years, there has been a strong demand to improve the functionality of toners while increasing carbon neutrality, including the aforementioned biomass-derived resins. However, if the biomass content of the toner is increased by components other than the release agent, such as a binder resin, the absolute value ΔSP, which is the difference between the dissolution parameter of the amorphous polyester resin and the dissolution parameter of the crystalline resin, increases, which can worsen compatibility and lead to poor low-temperature fixability. On the other hand, if low-temperature fixability is desired, the strength of the toner decreases, and photoreceptor filming may occur. Therefore, there has been a problem in that it is difficult to simultaneously use renewable resources and contribute to carbon neutrality, while also satisfying the low-temperature fixability and filming resistance required as toner characteristics.
[0026] In response to the aforementioned problem, the resin particles of the present invention are resin particles containing at least a binder resin, wherein the binder resin consists of an amorphous polyester resin and a crystalline resin, the alcohol monomer of the amorphous polyester resin contains propylene glycol, the proportion of the crystalline resin in the region within 150 nm from the outermost surface of the resin particles is 4% or less of the total amount of the resin particles, and radioactive carbon isotopes 14 By setting the C concentration to 5.4 pMC or higher, a significant contribution to carbon neutrality is achieved, along with excellent low-temperature fixation and filming resistance.
[0027] <Binding resin> The binder resin consists of an amorphous polyester resin and a crystalline resin.
[0028] <<Amorphous polyester resin>> The amorphous polyester resin contains propylene glycol as its alcohol monomer. Preferably, the propylene glycol is plant-derived. The inclusion of plant-derived components in the amorphous polyester resin enhances its carbon neutrality.
[0029] The amorphous polyester resin is not particularly limited as long as its alcohol monomer contains propylene glycol, and can be appropriately selected depending on the purpose. However, it is preferable that it contains amorphous polyester resin B, which is described below, and it is even more preferable that it contains both amorphous polyester resin A and amorphous polyester resin B.
[0030] <<<Amorphous polyester resin A>>> The amorphous polyester resin A is not particularly limited and can be appropriately selected depending on the purpose, but it is preferably one with a glass transition temperature (Tg) of -60°C or higher and 20°C or lower, and more preferably one with a glass transition temperature (Tg) of -40°C or higher and 20°C or lower. Furthermore, it is preferably obtained by the reaction of a nonlinear reactive precursor with a curing agent.
[0031] Furthermore, the amorphous polyester resin A preferably has at least one of urethane bonds and urea bonds, as this provides superior adhesion to recording media such as paper. By having either urethane bonds or urea bonds, the amorphous polyester resin A exhibits behavior similar to that of a pseudo-crosslinking point, thereby enhancing the rubbery properties of the amorphous polyester resin A and improving the heat resistance and high-temperature offset resistance of the resin particles.
[0032] -Nonlinear reactive precursors- The nonlinear reactive precursor is not particularly limited as long as it is a polyester resin (hereinafter sometimes referred to as "prepolymer") having a group that can react with the curing agent, and can be appropriately selected depending on the purpose.
[0033] There are no particular limitations on the groups in the prepolymer that can react with the curing agent, and they can be appropriately selected depending on the purpose. For example, groups that can react with active hydrogen groups can be used. Examples of groups that can react with the active hydrogen group include isocyanate groups, epoxy groups, carboxylic acids, or acid chloride groups. Among these, isocyanate groups are preferred as groups that can react with the active hydrogen group because they can introduce urethane bonds or urea bonds into the amorphous polyester resin A.
[0034] The prepolymer is preferably nonlinear. Nonlinear means having a branched structure conferred by at least one of a trivalent or higher alcohol and a trivalent or higher carboxylic acid. Furthermore, a polyester resin containing isocyanate groups is preferred as the prepolymer.
[0035] The polyester resin containing the isocyanate group is not particularly limited and can be appropriately selected depending on the purpose. Examples include reaction products of a polyester resin having an active hydrogen group and a polyisocyanate.
[0036] --Polyester resin containing active hydrogen groups-- There are no particular limitations on the polyester resin having the active hydrogen group, and it can be appropriately selected depending on the purpose. For example, one could be obtained by polycondensation of a polyhydric alcohol and a polyhydric carboxylic acid.
[0037] ---Polyhydric alcohol--- The polyhydric alcohol is not particularly limited and can be appropriately selected depending on the purpose. Examples include diols, trihydric or higher alcohols, or mixtures of diols and trihydric or higher alcohols. These may be used individually or in combination of two or more. The trihydric or higher alcohol imparts a branched structure to the polyester resin containing the isocyanate group.
[0038] The aforementioned diol is not particularly limited and can be appropriately selected depending on the purpose. Examples include aliphatic diols, diols having an oxyalkylene group, alicyclic diols, alkylene oxide adducts of alicyclic diols, bisphenols, or alkylene oxide adducts of bisphenols. Examples of the aliphatic diol include ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,4-butanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, 1,8-octanediol, 1,10-decanediol, or 1,12-dodecanediol. Examples of diols having an oxyalkylene group include diethylene glycol, triethylene glycol, dipropylene glycol, polyethylene glycol, polypropylene glycol, or polytetramethylene glycol. Examples of the alicyclic diol include 1,4-cyclohexanedimethanol or hydrogenated bisphenol A. Examples of alkylene oxide adducts of the alicyclic diol include those obtained by adding an alkylene oxide such as ethylene oxide, propylene oxide, or butylene oxide to the alicyclic diol. Examples of the bisphenols mentioned above include bisphenol A, bisphenol F, or bisphenol S. Examples of alkylene oxide adducts of the bisphenols include those obtained by adding an alkylene oxide such as ethylene oxide, propylene oxide, or butylene oxide to the bisphenols. These may be used individually or in combination of two or more types. Among these, aliphatic diols having 4 to 12 carbon atoms are preferred as the diol.
[0039] There are no particular restrictions on the trivalent or higher alcohols, and they can be appropriately selected depending on the purpose. Examples include trivalent or higher aliphatic alcohols, trivalent or higher polyphenols, or alkylene oxide adducts of trivalent or higher polyphenols. Examples of the aliphatic alcohols with a valency of 3 or higher include glycerin, trimethylolethane, trimethylolpropane, pentaerythritol, or sorbitol. Examples of the aforementioned polyphenols with a valency of 3 or higher include trisphenol PA, phenol novolac, or cresol novolac. Examples of alkylene oxide adducts of polyphenols with a valency of 3 or higher include those obtained by adding an alkylene oxide such as ethylene oxide, propylene oxide, or butylene oxide to polyphenols with a valency of 3 or higher. These may be used individually or in combination of two or more types.
[0040] The amorphous polyester resin A preferably contains the trivalent or higher aliphatic alcohol as a constituent component. The inclusion of the trivalent or higher aliphatic alcohol as a constituent component of the amorphous polyester resin A results in a branched structure within its molecular framework and a three-dimensional network structure of molecular chains, giving it rubber-like properties such as deformation at low temperatures but non-flow. Therefore, the heat resistance and high-temperature offset resistance of the resin particles can be maintained.
[0041] Furthermore, in order to lower the glass transition temperature (Tg) of the amorphous polyester resin A and to facilitate the property of deforming at low temperatures, it is preferable that the amorphous polyester resin A contains a diol component as a constituent, and that the total alcohol component in the amorphous polyester resin A contains 50 mol% or more of aliphatic diols having 4 to 12 carbon atoms.
[0042] ---Polyhydric carboxylic acids--- The polycarboxylic acid is not particularly limited and can be appropriately selected depending on the purpose. Examples include dicarboxylic acids, trivalent or higher carboxylic acids, or mixtures of dicarboxylic acids and trivalent or higher carboxylic acids. These may be used individually or in combination of two or more. The trivalent or higher carboxylic acid imparts a branched structure to the polyester resin containing the isocyanate group.
[0043] The dicarboxylic acid is not particularly limited and can be appropriately selected depending on the purpose. Examples include aliphatic dicarboxylic acids, aromatic dicarboxylic acids, their anhydrides, their lower (1-3 C1) alkyl esters, or their halides. These may be used individually or in combination of two or more.
[0044] The aliphatic dicarboxylic acid is not particularly limited and can be appropriately selected depending on the purpose. Examples include succinic acid, adipic acid, sebacic acid, dodecanediic acid, maleic acid, or fumaric acid.
[0045] The aromatic dicarboxylic acid is not particularly limited and can be appropriately selected depending on the purpose, but aromatic dicarboxylic acids having 8 to 20 carbon atoms are preferred. The aromatic dicarboxylic acid having 8 to 20 carbon atoms is not particularly limited and can be appropriately selected depending on the purpose, and examples include phthalic acid, isophthalic acid, terephthalic acid, or naphthalenedicarboxylic acid.
[0046] The carboxylic acid with a valency of 3 or higher is not particularly limited and can be appropriately selected depending on the purpose. Examples include aromatic carboxylic acids with a valency of 3 or higher, their anhydrides, their lower (1-3 C1) alkyl esters, or their halides. These may be used individually or in combination of two or more.
[0047] There are no particular restrictions on the trivalent or higher aromatic carboxylic acid, and it can be appropriately selected depending on the purpose, but trivalent or higher aromatic carboxylic acids having 9 to 20 carbon atoms are preferred. Examples of the aforementioned trivalent or higher aromatic carboxylic acids having 9 to 20 carbon atoms include trimellitic acid and pyromellitic acid.
[0048] Among these, the polycarboxylic acid preferably includes succinic acid, sebacic acid, or dodecanediic acid, which are saturated aliphatic compounds derived from plants. The plant origin of the polycarboxylic acid enhances carbon neutrality. The saturated aliphatic compounds have the effect of increasing the recrystallization properties of the crystalline resin, thereby increasing the aspect ratio of the crystalline resin and improving its low-temperature fixability.
[0049] In order to lower the glass transition temperature (Tg) and make it easier to impart the property of deforming at low temperatures, the amorphous polyester resin A preferably contains a dicarboxylic acid component as a constituent of the amorphous polyester resin A, and preferably contains 50 mol% or more of aliphatic dicarboxylic acid having 4 to 12 carbon atoms in the total acid component of the amorphous polyester resin A.
[0050] --Polyisocyanate-- There are no particular restrictions on the polyisocyanate, and it can be appropriately selected depending on the purpose. Examples include diisocyanates or polyisocyanates with a valent or higher nucleotide
[0051] The diisocyanate is not particularly limited and can be appropriately selected depending on the purpose. Examples include aliphatic diisocyanates, alicyclic diisocyanates, aromatic diisocyanates, aromatic aliphatic diisocyanates, or isocyanurates, or those blocked with phenol derivatives, oximes, caprolactams, etc.
[0052] Examples of the aliphatic diisocyanates include tetramethylene diisocyanate, hexamethylene diisocyanate, methyl 2,6-diisocyanatocaproate, octamethylene diisocyanate, decamethylene diisocyanate, dodecamethylene diisocyanate, tetradecamethylene diisocyanate, trimethylhexane diisocyanate, or tetramethylhexane diisocyanate.
[0053] Examples of the alicyclic diisocyanate include isophorone diisocyanate or cyclohexylmethane diisocyanate.
[0054] Examples of the aromatic diisocyanates include tolylene diisocyanate, diisocyanatodiphenylmethane, 1,5-naphthylene diisocyanate, 4,4'-diisocyanatodiphenyl, 4,4'-diisocyanato-3,3'-dimethyldiphenyl, 4,4'-diisocyanato-3-methyldiphenylmethane, or 4,4'-diisocyanato-diphenyl ether.
[0055] Examples of the aforementioned aromatic aliphatic diisocyanates include α,α,α',α'-tetramethylxylylene diisocyanate.
[0056] Examples of the isocyanurates include tris(isocyanatoalkyl)isocyanurate or tris(isocyanatocycloalkyl)isocyanurate.
[0057] Examples of the aforementioned trivalent or higher polyisocyanates include lysine triisocyanate or diisocyanate-modified alcohols with a trivalent or higher hydration.
[0058] -Hardening agent- The curing agent is not particularly limited as long as it reacts with the nonlinear reactive precursor to produce the amorphous polyester resin A, and can be appropriately selected depending on the purpose. Examples include active hydrogen group-containing compounds.
[0059] --Compounds containing active hydrogen groups-- There are no particular restrictions on the active hydrogen group in the active hydrogen group-containing compound, and it can be appropriately selected depending on the purpose. Examples include hydroxyl groups (alcoholic hydroxyl groups and phenolic hydroxyl groups), amino groups, carboxyl groups, or mercapto groups. These may be used individually or in combination of two or more.
[0060] The active hydrogen group-containing compound is not particularly limited and can be appropriately selected depending on the purpose, but amines are preferred because they can form urea bonds.
[0061] There are no particular restrictions on the amines, and they can be appropriately selected depending on the purpose. Examples include diamines, trivalent or higher amines, amino alcohols, amino mercaptans, amino acids, or those in which the amino group has been blocked. These may be used individually or in combination of two or more. Among these, diamines or mixtures of diamines and small amounts of trivalent or higher amines are preferred.
[0062] The diamine is not particularly limited and can be appropriately selected depending on the purpose. Examples include aromatic diamines, alicyclic diamines, or aliphatic diamines.
[0063] The aromatic diamine is not particularly limited and can be appropriately selected depending on the purpose. Examples include phenylenediamine, diethyltoluenediamine, or 4,4'-diaminodiphenylmethane.
[0064] The alicyclic diamine is not particularly limited and can be appropriately selected depending on the purpose. Examples include 4,4'-diamino-3,3'-dimethyldicyclohexylmethane, diaminocyclohexane, or isophorone diamine.
[0065] The aliphatic diamine is not particularly limited and can be appropriately selected depending on the purpose. Examples include ethylenediamine, tetramethylenediamine, or hexamethylenediamine.
[0066] There are no particular restrictions on the amine with a valency of 3 or higher, and it can be appropriately selected depending on the purpose. Examples include diethylenetriamine and triethylenetetramine.
[0067] The amino alcohol is not particularly limited and can be appropriately selected depending on the purpose. Examples include ethanolamine or hydroxyethylaniline.
[0068] The amino mercaptan is not particularly limited and can be appropriately selected depending on the purpose. Examples include aminoethyl mercaptan or aminopropyl mercaptan.
[0069] The aforementioned amino acid is not particularly limited and can be appropriately selected depending on the purpose; for example, aminopropionic acid or aminocaproic acid can be used.
[0070] There are no particular limitations on the amino group that is blocked, and it can be appropriately selected depending on the purpose. Examples include ketimine compounds or oxazoline compounds obtained by blocking the amino group with ketones such as acetone, methyl ethyl ketone, and methyl isobutyl ketone.
[0071] The weight-average molecular weight (Mw) of the amorphous polyester resin A is not particularly limited and can be appropriately selected depending on the purpose. However, as measured by gel permeation chromatography (GPC), it is preferably 10,000 to 1,000,000, more preferably 10,000 to 300,000, and particularly preferably 10,000 to 200,000. When the weight-average molecular weight is 10,000 or more, it is possible to suppress the flow of the resin particles at low temperatures and improve heat resistance for storage. It is also possible to suppress a decrease in viscosity during melting and suppress a decrease in high-temperature offset properties.
[0072] The molecular structure of the amorphous polyester resin A can be determined by nuclear magnetic resonance spectroscopy (NMR) in solution or solid state, as well as by X-ray diffraction, gas chromatography-mass spectrometry (GC / MS), liquid chromatography-mass spectrometry (LC / MS), or infrared absorption spectroscopy (IR). Among these, the infrared absorption spectrum obtained by IR is 965±10 cm⁻¹. -1 and 990±10cm -1 One method for detecting amorphous polyester resins that do not exhibit absorption based on δCH (out-of-plane angular bending vibration) of olefins is to identify them as such.
[0073] There are no particular restrictions on the content of the amorphous polyester resin A, and it can be appropriately selected depending on the purpose, but it is preferably 5 to 25 parts by mass, and more preferably 10 to 20 parts by mass, per 100 parts by mass of the resin particles. When the content of the amorphous polyester resin A is 5 parts by mass or more per 100 parts by mass of the resin particles, deterioration of low-temperature fixing properties and high-temperature offset resistance can be suppressed. Furthermore, when the content of the amorphous polyester resin A is 25 parts by mass or less per 100 parts by mass of the resin particles, deterioration of heat-resistant storage and a decrease in the glossiness of the image obtained after fixing can be suppressed. When the content of the amorphous polyester resin A is within the more preferable range described above, it is advantageous in that it is excellent in all aspects of low-temperature fixing properties, high-temperature offset resistance, and heat-resistant storage.
[0074] <<<Amorphous polyester resin B>>> The amorphous polyester resin B is preferably a linear polyester resin, and more preferably an unmodified polyester resin. The aforementioned unmodified polyester resin is a polyester resin obtained using a polyhydric alcohol and a polyhydric carboxylic acid or its derivative, and is not modified by an isocyanate compound or the like. The amorphous polyester resin B is preferably free from urethane and urea bonds.
[0075] -Polyhydric alcohols- There are no particular restrictions on the polyhydric alcohols, and they can be appropriately selected depending on the purpose. Examples include diols. Examples of the aforementioned diols include alkylene (2-3 carbon atoms) oxide (average number of added moles 1-10) adducts of bisphenol A, ethylene glycol, propylene glycol, neopentyl glycol, hydrogenated bisphenol A, or alkylene (2-3 carbon atoms) oxide (average number of added moles 1-10) adducts of hydrogenated bisphenol A. Examples of the alkylene (2-3 carbon atoms) oxide (average number of added moles 1-10) adducts of bisphenol A include polyoxypropylene (2.2)-2,2-bis(4-hydroxyphenyl)propane or polyoxyethylene (2.2)-2,2-bis(4-hydroxyphenyl)propane. These may be used individually or in combination of two or more. Among these, it is preferable that the polyhydric alcohol includes plant-derived ethylene glycol or propylene glycol. The plant-derived nature of the polyhydric alcohol enhances carbon neutrality.
[0076] Furthermore, for the purpose of adjusting the acid value and hydroxyl value, the amorphous polyester resin B may contain trivalent or higher alcohols at the ends of its resin chains. Examples of trivalent or higher alcohols include glycerin, pentaerythritol, or trimethylolpropane.
[0077] -Polycarboxylic acids or their derivatives- The polycarboxylic acid is not particularly limited and can be appropriately selected depending on the purpose; for example, dicarboxylic acids can be used. Examples of the dicarboxylic acid include adipic acid, phthalic acid, isophthalic acid, terephthalic acid, fumaric acid, maleic acid, succinic acid, succinic acid substituted with an alkyl group having 1 to 20 carbon atoms or an alkenyl group having 2 to 20 carbon atoms, or modified purified rosin. Examples of succinic acid substituted with the aforementioned C1-C20 alkyl group or C2-C20 alkenyl group include dodecenyl succinic acid or octyl succinic acid. There are no particular limitations on the derivative of the polycarboxylic acid, and it can be appropriately selected depending on the purpose. Examples include polycarboxylic acid anhydrides and polycarboxylic acid esters. The modified purified rosin is preferably one modified with, for example, acrylic acid, fumaric acid, or maleic acid. These can be used individually or in combination of two or more.
[0078] Among these, it is preferable that the polycarboxylic acid includes succinic acid, a saturated aliphatic acid derived from plants. The plant origin of the polycarboxylic acid enhances carbon neutrality.
[0079] The amorphous polyester resin B preferably contains a dicarboxylic acid component, and the dicarboxylic acid component preferably contains 50 mol% or more of terephthalic acid. This is advantageous in terms of heat resistance and storage properties.
[0080] Furthermore, for the purpose of adjusting the acid value and hydroxyl value, the amorphous polyester resin B may contain trivalent or higher carboxylic acids at the ends of its resin chains. Examples of the carboxylic acids with a valency of 3 or higher include trimellitic acid, pyromellitic acid, or their acid anhydrides.
[0081] There are no particular restrictions on the molecular weight of the amorphous polyester resin B, and it can be appropriately selected depending on the purpose, but it is preferable that it is within the following range when measured by gel permeation chromatography (GPC). The weight-average molecular weight (Mw) of the amorphous polyester resin B is preferably 3,000 to 10,000, and more preferably 4,000 to 10,000. The number-average molecular weight (Mn) of the amorphous polyester resin B is preferably 1,000 to 4,000, and more preferably 1,500 to 3,000. The molecular weight ratio (Mw / Mn) of the amorphous polyester resin B is preferably 1.0 to 4.0, and more preferably 1.0 to 3.5. When the weight-average molecular weight (Mw) and number-average molecular weight (Mn) of the amorphous polyester resin B are above the lower limit of the preferred range, it is possible to suppress a decrease in the heat-resistant storage properties of the resin particles and their durability against stress such as agitation in the developing machine. Furthermore, when the weight-average molecular weight (Mw) and number-average molecular weight (Mn) of the amorphous polyester resin B are below the upper limit of the preferred range, it is possible to suppress an increase in the viscoelasticity of the resin particles when melted and suppress a decrease in low-temperature fixability.
[0082] There are no particular restrictions on the acid value of the amorphous polyester resin B, and it can be appropriately selected depending on the purpose, but 1 mg KOH / g to 50 mg KOH / g is preferred, and 5 mg KOH / g to 30 mg KOH / g is more preferred. When the acid value of the amorphous polyester resin B is 1 mg KOH / g or higher, the toner containing the resin particles tends to become negatively charged, and furthermore, when fixed to a recording medium such as paper, the affinity between the recording medium and the toner improves, and low-temperature fixing performance can be improved. In addition, when the acid value of the amorphous polyester resin B is 50 mg KOH / g or lower, it is possible to suppress a decrease in charge stability, especially charge stability against environmental fluctuations. The acid value of the amorphous polyester resin B can be measured in accordance with the measurement method described in JIS K0070-1992.
[0083] The hydroxyl value of the amorphous polyester resin B is not particularly limited and can be appropriately selected depending on the purpose, but it is preferably 5 mg KOH / g or higher. Furthermore, the upper limit of the hydroxyl value of the amorphous polyester resin B is not particularly limited and can be appropriately selected depending on the purpose, but it is preferably 30 mg KOH / g or lower. The lower and upper limits of the hydroxyl value of the amorphous polyester resin B can be appropriately combined, with 5 mg KOH / g to 30 mg KOH / g being preferred. The hydroxyl value of the amorphous polyester resin B can be measured in accordance with the measurement method described in JIS K0070-1966.
[0084] There are no particular restrictions on the glass transition temperature (Tg) of the amorphous polyester resin B, and it can be appropriately selected depending on the purpose, but it is preferably 40°C to 80°C, and more preferably 50°C to 70°C. When the glass transition temperature (Tg) of the amorphous polyester resin B is 40°C or higher, the heat resistance and durability against stress such as agitation in the developing machine of the toner containing the resin particles are sufficient, and the filming resistance is also good. When the glass transition temperature (Tg) of the amorphous polyester resin B is 80°C or lower, the deformation due to heating and pressurization during the fixing of the toner containing the resin particles is sufficient, and the low-temperature fixing performance is good.
[0085] The molecular structure of the amorphous polyester resin B can be determined by nuclear magnetic resonance spectroscopy (NMR) in solution or solid state, as well as by X-ray diffraction, gas chromatography-mass spectrometry (GC / MS), liquid chromatography-mass spectrometry (LC / MS), or infrared absorption spectroscopy (IR). Among these, the infrared absorption spectrum obtained by IR is 965±10 cm⁻¹. -1 and 990±10cm -1 One method for detecting amorphous polyester resin B is one in which the material does not have absorption based on δCH (out-of-plane angular bending vibration) of the olefin.
[0086] There are no particular restrictions on the content of the amorphous polyester resin B, and it can be appropriately selected depending on the purpose, but it is preferably 45 to 90 parts by mass, and more preferably 60 to 80 parts by mass, per 100 parts by mass of the resin particles. When the content of the amorphous polyester resin B is 45 parts by mass or more per 100 parts by mass of the resin particles, deterioration of the dispersibility of the pigment or release agent in the resin particles can be suppressed, and the occurrence of image fogging or distortion can be suppressed. Furthermore, when the content of the amorphous polyester resin B is 90 parts by mass or less per 100 parts by mass of the resin particles, the content of the crystalline resin and the amorphous polyester resin A can be prevented from decreasing, and a decrease in low-temperature fixability can be suppressed. When the content of the amorphous polyester resin B is within the more preferable range, it is advantageous in that it is excellent in both high image quality and low-temperature fixability.
[0087] <<Crystalline resin>> The crystalline resin is not particularly limited as long as it has crystalline properties and can be appropriately selected according to the purpose. Examples include polyester resin, polyurethane resin, polyurea resin, polyamide resin, polyether resin, vinyl resin, or modified crystalline resin. These may be used individually or in combination of two or more. Among these, crystalline polyester resin is preferred as the crystalline resin.
[0088] -Crystalline polyester resin- The aforementioned crystalline polyester resin (hereinafter sometimes referred to as "crystalline polyester resin C") exhibits thermal melting properties in which its viscosity changes rapidly near the fixing start temperature due to its high crystallinity.
[0089] By using the crystalline polyester resin C having such properties together with the amorphous polyester resin, resin particles possessing both good heat resistance and low-temperature fixation properties can be obtained. For example, by using the crystalline polyester resin C and the amorphous polyester resin in combination, the crystalline properties of the crystalline polyester resin C provide good heat resistance until just before the melting start temperature. At the melting start temperature, the crystalline polyester resin C undergoes a rapid decrease in viscosity (sharp melt property) due to melting, and consequently becomes compatible with the amorphous polyester resin B, allowing for good fixation as both rapidly decrease in viscosity. Furthermore, good results are also shown regarding the release width (the difference between the lower limit temperature for fixation and the temperature at which high-temperature offset occurs).
[0090] The crystalline polyester resin C is obtained using a polyhydric alcohol and a polyhydric carboxylic acid or its derivative. Furthermore, by using a plant-derived compound in at least one of the polyhydric alcohol and the polyhydric carboxylic acid or its derivative, the crystalline resin can be made a biomass-derived resin. These may be used individually or in combination of two or more.
[0091] There are no particular limitations on the derivative of the polycarboxylic acid, and it can be appropriately selected depending on the purpose. Examples include polycarboxylic acid anhydrides or polycarboxylic acid esters.
[0092] In this specification, the crystalline polyester resin C refers to a resin obtained using the polyhydric alcohol and the polyhydric carboxylic acid or its derivative, as described above. Modified polyester resins, such as the prepolymer, and resins obtained by subjecting the prepolymer to at least one of a crosslinking reaction and an extension reaction, do not belong to the crystalline polyester resin C.
[0093] --Polyhydric alcohols-- There are no particular restrictions on the polyhydric alcohols, and they can be appropriately selected depending on the purpose. Examples include diols or alcohols with a hydride of three or more. Examples of the aforementioned diols include saturated aliphatic diols. Examples of the saturated aliphatic diol include linear saturated aliphatic diols and branched saturated aliphatic diols. Among these, linear saturated aliphatic diols are preferred, and linear saturated aliphatic diols with 2 to 12 carbon atoms are more preferred. A linear saturated aliphatic diol is preferable because it results in high crystallinity and a high melting point for the crystalline polyester resin C. However, if the number of carbon atoms in the saturated aliphatic diol exceeds 12, it becomes difficult to obtain practical materials. It is more preferable that the number of carbon atoms in the saturated aliphatic diol be 12 or less.
[0094] Specific examples of the saturated aliphatic diols include ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 1,13-tridecanediol, 1,14-tetradecanediol, 1,18-octadecanediol, or 1,14-eicosandecanediol. These may be used individually or in combination of two or more. Among these, ethylene glycol, 1,4-butanediol, 1,6-hexanediol, 1,8-octanediol, 1,10-decanediol, or 1,12-dodecanediol are preferred because the crystalline polyester resin C has high crystallinity and excellent sharp-melt properties.
[0095] Examples of trivalent or higher alcohols include glycerin, trimethylolethane, trimethylolpropane, or pentaerythritol. These may be used individually or in combination of two or more.
[0096] --Polyhydric carboxylic acids-- The polycarboxylic acid is not particularly limited and can be appropriately selected depending on the purpose; for example, dicarboxylic acids can be used. Examples of the dicarboxylic acid include saturated aliphatic dicarboxylic acids, unsaturated aliphatic dicarboxylic acids, or aromatic dicarboxylic acids. Examples of the saturated aliphatic dicarboxylic acid include oxalic acid, malonic acid, succinic acid, glutaric acid, sebacic acid, adipic acid, or dodecanediic acid. Examples of the aforementioned unsaturated aliphatic dicarboxylic acid include fumaric acid and maleic acid. Examples of the saturated aliphatic dicarboxylic acid include terephthalic acid. These can be used individually or in combination of two or more types.
[0097] The dicarboxylic acid is preferably a saturated aliphatic compound of plant origin with 4 to 12 carbon atoms, and more preferably sebacic acid of plant origin. The plant origin of the dicarboxylic acid enhances carbon neutrality. When the dicarboxylic acid has 12 or fewer carbon atoms, its compatibility with the amorphous polyester resin improves, increasing the aspect ratio of the crystalline polyester resin and improving low-temperature fixability. Furthermore, saturated aliphatic compounds enhance the recrystallization properties of the crystalline polyester resin C, increasing its aspect ratio and improving low-temperature fixability.
[0098] There are no particular restrictions on the melting point of the crystalline polyester resin C, and it can be appropriately selected depending on the purpose, but it is preferably 60°C or higher and 80°C or lower. If the melting point of the crystalline polyester resin C is 60°C or higher, it is possible to suppress the melting of the crystalline polyester resin C at low temperatures, which would reduce the heat-resistant storage properties of the resin particles. Furthermore, if the melting point of the crystalline polyester resin C is 80°C or lower, it is possible to improve the melting of the crystalline polyester resin C due to heating during fixing, and suppress the decrease in low-temperature fixing properties.
[0099] There are no particular restrictions on the molecular weight of the crystalline polyester resin C, and it can be appropriately selected depending on the purpose. However, from the viewpoint that a sharp molecular weight distribution and low molecular weight resins have excellent low-temperature fixation properties, and a high proportion of high molecular weight components improves heat resistance and storage properties, it is preferable that the molecular weight of the soluble orthodichlorobenzene in the crystalline polyester resin C measured by gel permeation chromatography (GPC) is within the following range. The weight-average molecular weight (Mw) of the crystalline polyester resin C is preferably 3,000 to 30,000, and more preferably 5,000 to 20,000. The number-average molecular weight (Mn) of the crystalline polyester resin C is preferably 1,000 to 10,000, and more preferably 2,000 to 10,000. The molecular weight ratio (Mw / Mn) of the crystalline polyester resin C is preferably 1.0 to 10, and more preferably 1.0 to 5.0.
[0100] There are no particular restrictions on the acid value of the crystalline polyester resin C, and it can be appropriately selected depending on the purpose. However, the lower limit of the oxidation value is preferably 5 mg KOH / g or higher, and more preferably 10 mg KOH / g or higher, from the viewpoint of affinity between the recording medium and the resin particles, in order to achieve the desired low-temperature fixation properties. Furthermore, the upper limit of the acid value of the crystalline polyester resin C is preferably 45 mg KOH / g or lower, from the viewpoint of improving resistance to high-temperature offset properties. The oxidation of the crystalline polyester resin C can be measured in accordance with the measurement method described in JIS K0070-1992.
[0101] The hydroxyl value of the crystalline polyester resin C is not particularly limited and can be appropriately selected depending on the purpose. However, in order to achieve the desired low-temperature fixability and good electrostatic properties, a value of 0 mg KOH / g or more and 50 mg KOH / g or less is preferred, and 5 mg KOH / g or more and 10 mg KOH / g or less is more preferred. The hydroxyl value of the crystalline polyester resin C can be measured in accordance with the measurement method described in JIS K0070-1966.
[0102] The molecular structure of the crystalline polyester resin C can be determined by nuclear magnetic resonance spectroscopy (NMR) in solution or solid state, as well as by X-ray diffraction, gas chromatography-mass spectrometry (GC / MS), liquid chromatography-mass spectrometry (LC / MS), or infrared absorption spectroscopy (IR). Among these, the infrared absorption spectrum obtained by IR is 965±10 cm⁻¹. -1 and 990±10cm -1 A simple method for detecting the crystalline polyester resin C that has absorption based on the δCH (out-of-plane bending vibration) of the olefin is to identify it as such.
[0103] There are no particular restrictions on the content of the crystalline polyester resin C in the resin particles, and it can be appropriately selected depending on the purpose, but preferably it is 3 to 20 parts by mass, and more preferably 5 to 15 parts by mass, per 100 parts by mass of the resin particles. When the content of the crystalline polyester resin C in the resin particles is 3 parts by mass or more, the sharp melting by the crystalline polyester resin C can be improved, and the low-temperature fixing properties can be improved. Furthermore, when the content of the crystalline polyester resin C in the resin particles is 20 parts by mass or less, the decrease in heat resistance and the occurrence of image fogging can be suppressed. When the content of the crystalline polyester resin C in the resin particles is within the more preferable range, it is advantageous in that it is excellent in both high image quality and low-temperature fixing properties.
[0104] There are no particular restrictions on the major axis of the crystalline resin, and it can be appropriately selected depending on the purpose, but it is preferably 500 nm or less, and more preferably 300 nm or less. When the major axis of the crystalline resin is 500 nm or less, the crystalline resin is less likely to be exposed on the surface of the resin particles, and the filming resistance is improved.
[0105] There are no particular restrictions on the aspect ratio of the crystalline resin, and it can be appropriately selected depending on the purpose, but a ratio of 4.0 or higher is preferred, and a ratio of 10.0 or higher is more preferred. When the aspect ratio of the crystalline resin is 4.0 or higher, the contact area with the amorphous polyester resin increases, the compatibility between the amorphous polyester resin and the crystalline resin during fixing improves, and the low-temperature fixing performance improves.
[0106] The major axis and aspect ratio of the crystalline resin in the resin particles can be measured, for example, by the following method. The resin particles are embedded in epoxy resin (S-31, manufactured by DEVCON), cut to a thickness of 60 nm using an ultrasonic ultramicrotome (Leica EM UC7, manufactured by Leica), and stained with ruthenium using a vacuum staining device (manufactured by Philgen Co., Ltd.). Subsequently, observation is performed using a transmission electron microscope (H-7500, manufactured by Hitachi High-Tech Corporation) at an acceleration voltage of 120 kV. At this time, 50 resin particles are arbitrarily selected from those within ±2.0 μm of the weight-average particle size of the resin particles and photographed. As described above, in the configuration of the present invention, when RuO4 staining is performed, the density of the crystalline resin in the resin particles is projected more intensely. The average major axis and average aspect ratio of the domains made up of the crystalline resin can be measured from the observed image, but may also be calculated using image processing software if necessary.
[0107] Image-Pro Plus 5.1 can be used as the image processing software. The method for calculating the average major axis and average aspect ratio of the crystalline resin using Image-Pro Plus 5.1 is as follows. (1) Use the cross-sectional image of the resin particles taken using the method described above. First, in order to extract the resin particles to be analyzed, select the resin particle portion to separate the resin particles from the background. (2) Select "Measurement" - "Count / Size" in Image-Pro Plus 5.1. From the "Count / Size" window, select "Measurement" - "Measurement Item". Select "Diameter (Minimum)" and "Diameter (Maximum)" from the measurement items. In "Brightness Range Selection", it is necessary to adjust the brightness range so that only the crystalline resin in each resin particle selected in (1) above is selected. Depending on the RuO4 staining conditions, the brightness range may need to be changed each time, but the difference in density as described above makes it easy to distinguish the crystalline resin. Select "Count" to display the measurement results. (3) The "maximum diameter" obtained in (2) above is the major axis of the crystalline resin. Also, the aspect ratio (major axis / minor axis) can be determined by taking the "minimum diameter" obtained in (2) above as the minor axis and the "maximum diameter" as the major axis. (4) From the data of the major axis and aspect ratio of each crystalline resin in a single resin particle obtained in (1) to (3) above, the average value of 10 points is calculated in descending order of "diameter (maximum)". (5) Repeat the operations in (1) to (4) above for 50 resin particles to calculate the average length and average aspect ratio of the 50 resin particles. These average values are taken as the average length and average aspect ratio of the crystalline resin in the resin particles in the present invention.
[0108] When amorphous polyester resin A, amorphous polyester resin B, and crystalline polyester resin C are used in combination in the aforementioned resin particles, extremely excellent low-temperature fixability is achieved. Furthermore, in order to achieve both low-temperature fixability and high-temperature, high-humidity storage properties, it is preferable that the amorphous polyester resin A has a very low glass transition temperature. When the amorphous polyester resin A has a very low glass transition temperature, it has the property of deforming at low temperatures, deforming in response to heating and pressurization during fixation, and having the property of adhering more easily to recording media such as paper at lower temperatures. In addition, in one embodiment of the amorphous polyester resin A, since the reactive precursor is nonlinear, it has a branched structure in the molecular backbone, and the molecular chains form a three-dimensional network structure, so it deforms at low temperatures but does not flow, thus having rubber-like properties. Therefore, even when the glass transition temperature is set lower than that of conventional toners, it is possible to maintain the heat resistance and high-temperature offset resistance of the toner containing the resin particles, and by lowering the glass transition temperature of the toner, excellent low-temperature fixability is achieved.
[0109] Furthermore, if the amorphous polyester resin A has urethane or urea bonds with high cohesive energy, its adhesion to recording media such as paper is improved. Also, since urethane or urea bonds behave like pseudo-crosslinking points, the rubber-like properties are enhanced, resulting in improved heat resistance and high-temperature offset resistance of the toner containing the resin particles.
[0110] <Other ingredients> The other components in the resin particles are not particularly limited and can be appropriately selected depending on the purpose. Examples include colorants, release agents, charge control agents, flow improvers, cleaning improvers, magnetic materials, or shape modifiers. These may be used individually or in combination of two or more.
[0111] <<Coloring agent>> There are no particular restrictions on the aforementioned colorants, and they can be appropriately selected according to the purpose. For example, carbon black, nigrosine dye, iron black, naphthol yellow S, Hansa yellow (10G, 5G, G), cadmium yellow, yellow iron oxide, yellow ochre, yellow lead, titanium yellow, polyazo yellow, oil yellow, Hansa yellow (GR, A, RN, R), pigment yellow L, benzidine yellow (G, GR), permanent yellow (NCG), Vulcan fast yellow (5G, R), tartrazine lake, quinoline yellow lake, anthrazane yellow BG L, Isoindolinone Yellow, Bengara, Red Lead, Red Lead, Cadmium Red, Cadmium Mercury Red, Antimony Red, Permanent Red 4R, Para Red, Faise Red, Parachloro-orthonitroaniline Red, Risol Fast Scarlet G, Brilliant Fast Scarlet, Brilliant Carmine BS, Permanent Red (F2R, F4R, FRL, FRLL, F4RH), Fast Scarlet VD, Belkan Fast Rubin B, Brilliant Scarlet G, Risol Rubin GX, Permanent Red F5R, Brillia Bon Maroon 6B, Pigment Scarlet 3B, Bordeaux 5B, Toluidine Maroon, Permanent Bordeaux F2K, Helio Bordeaux BL, Bordeaux 10B, Bon Maroon Light, Bon Maroon Medium, Eosin Lake, Rhodamine Lake B, Rhodamine Lake Y, Alizarin Lake, Thioindigo Red B, Thioindigo Maroon, Oil Red, Quinacridone Red, Pyrazolone Red, Polyazo Red, Chrome Vermilion, Benzidine Orange, Perinon Orange, Oil Orange, Cobalt Blue, Cerulean Blue, Alkali Blue Lake, Peacock Blue Lake, Victoria Blue Lake, Metal-free Phthalocyanine Blue, Phthalocyanine Blue, Fast Sky Blue, Indanthrene Blue (RS, BC), Indigo, Ultramarine, Prussian Blue, Anthraquinone Blue, Fast Violet B, Methyl Violet Lake, Cobalt Purple, Manganese Purple, Dioxane Violet, Anthraquinone Violet, Chrome Green, Zinc Green, Chromium Oxide, Pyridian, Emerald Green, Pigment Green B, Naphthol Green B, Green Gold, Acid Green Lake,Examples include malachite green lake, phthalocyanine green, anthraquinone green, titanium dioxide, zinc oxide, or lithobone. These may be used individually or in combination of two or more.
[0112] There are no particular restrictions on the content of the coloring agent in the resin particles, and it can be appropriately selected depending on the purpose, but it is preferably 1 to 15 parts by mass, and more preferably 3 to 10 parts by mass, per 100 parts by mass of the resin particles.
[0113] The aforementioned coloring agent can also be used as a masterbatch compounded with resin. The resin used in the production of the masterbatch or kneaded together with the masterbatch is not particularly limited and can be appropriately selected depending on the purpose. Examples include, in addition to the amorphous polyester resin, polymers of styrene or its substituted derivatives, styrene copolymers, polymethyl methacrylate, polybutyl methacrylate, polyvinyl chloride, polyvinyl acetate, polyethylene, polypropylene, polyester, epoxy resin, epoxy polyol resin, polyurethane, polyamide, polyvinyl butyral, polyacrylic acid resin, rosin, modified rosin, terpene resin, aliphatic or alicyclic hydrocarbon resin, aromatic petroleum resin, chlorinated paraffin, or paraffin wax. These may be used individually or in combination of two or more. Examples of polymers of styrene or its substituted derivatives include polystyrene, poly-p-chlorostyrene, or polyvinyltoluene. Examples of the styrene-based copolymers include styrene-p-chlorostyrene copolymer, styrene-propylene copolymer, styrene-vinyltoluene copolymer, styrene-vinylnaphthalene copolymer, styrene-methyl acrylate copolymer, styrene-ethyl acrylate copolymer, styrene-butyl acrylate copolymer, styrene-octyl acrylate copolymer, styrene-methyl methacrylate copolymer, styrene-ethyl methacrylate copolymer, styrene-butyl methacrylate copolymer, styrene-α-chloromethacrylate copolymer, styrene-acrylonitrile copolymer, styrene-vinylmethyl ketone copolymer, styrene-butadiene copolymer, styrene-isoprene copolymer, styrene-acrylonitrile-indene copolymer, styrene-maleic acid copolymer, or styrene-maleic acid ester copolymer.
[0114] There are no particular limitations on the method for producing the masterbatch, and it can be appropriately selected depending on the purpose. For example, one method involves mixing and kneading the resin for the masterbatch and the coloring agent under high shear force. In this case, an organic solvent can be used to enhance the interaction between the coloring agent and the resin. Another method, known as the flushing method, involves mixing and kneading an aqueous paste containing water from the coloring agent with the resin and an organic solvent to transfer the coloring agent to the resin side and remove the water and organic solvent components. This method is also preferably used because it allows the wet cake of the coloring agent to be used as is, eliminating the need for drying. A high-shear dispersion device such as a three-roll mill is preferably used for mixing and kneading.
[0115] <<Release agent>> The mold release agent is not particularly limited and can be appropriately selected from known ones. Examples include waxes or waxes, fatty acid amides, homopolymers or copolymers of polyacrylates, or crystalline polymers having long alkyl groups in their side chains. These may be used individually or in combination of two or more.
[0116] Examples of the aforementioned waxes include natural waxes, synthetic hydrocarbon waxes, and synthetic waxes. Examples of the aforementioned natural waxes include plant-based waxes, animal-based waxes, mineral-based waxes, and petroleum waxes. Examples of the aforementioned plant-based waxes include carnauba wax, cotton wax, or wood wax. Examples of the aforementioned animal-derived waxes include beeswax and lanolin. Examples of the aforementioned mineral waxes include ozokerite or cersine. Examples of the petroleum wax include paraffin, microcrystalline, or petrolatum. Examples of the synthetic hydrocarbon waxes include Fischer-Tropsch wax or polyethylene wax. Examples of the synthetic waxes include esters, ketones, or ethers.
[0117] Examples of the fatty acid amide include 12-hydroxystearic acid amide, stearic acid amide, phthalic anhydride, or chlorinated hydrocarbons.
[0118] Examples of the polyacrylate include poly-n-stearyl methacrylate or poly-n-lauryl methacrylate, which are low molecular weight crystalline polymer resins. Examples of the homopolymer or copolymer of the polyacrylate include a copolymer of n-stearyl acrylate and ethyl methacrylate.
[0119] Among these, plant-based waxes or ester waxes made from plant-derived materials are preferred as the mold release agent. The plant-derived nature of the mold release agent enhances carbon neutrality.
[0120] There are no particular restrictions on the melting point of the mold release agent, and it can be appropriately selected depending on the purpose, but a melting point of 60°C or higher and 80°C or lower is preferred. If the melting point of the mold release agent is 60°C or higher, it is possible to suppress the melting of the mold release agent at low temperatures, thereby suppressing a decrease in heat resistance for storage. Furthermore, if the melting point of the mold release agent is 80°C or lower, it is possible to suppress the occurrence of a fixing offset due to insufficient melting of the mold release agent when the resin has melted and is in the fixing temperature range, thereby suppressing the occurrence of image defects.
[0121] There are no particular restrictions on the content of the release agent in the resin particles, and it can be appropriately selected depending on the purpose. However, it is preferably 2 parts by mass or more and 10 parts by mass or less, and more preferably 3 parts by mass or more and 8 parts by mass or less, per 100 parts by mass of the resin particles. When the content of the release agent is 2 parts by mass or more, it is possible to suppress a decrease in high-temperature offset resistance and low-temperature fixing performance during fixing. When it is 10 parts by mass or less, it is possible to suppress a decrease in heat-resistant storage performance and suppress the occurrence of image fogging, etc. When the content of the release agent is within the more preferable range described above, it is advantageous in terms of improving image quality and fixing stability.
[0122] The mold release agent, like the crystalline resin, is preferably encapsulated within the resin particles, and its presence is low in the region within 150 nm from the outermost surface of the resin particles, in order to improve filming resistance.
[0123] <<Static Control Agent>> The aforementioned charge control agent is not particularly limited and can be appropriately selected depending on the purpose. Examples include nigrosine dyes, triphenylmethane dyes, chromium-containing metal complex dyes, molybdate chelate pigments, rhodamine dyes, alkoxyamines, quaternary ammonium salts (including fluorine-modified quaternary ammonium salts), alkylamides, elemental or compound phosphorus, elemental or compound tungsten, fluorine-based surfactants, metal salicylate salts, metal salts of salicylate derivatives, metal oxynaphthoate salts, phenolic condensates, azo pigments, boron complexes, or polymer compounds having functional groups (e.g., sulfonic acid groups, carboxyl groups, or quaternary ammonium salts). These may be used individually or in combination of two or more.
[0124] Specific examples of the aforementioned charge control agents include Bontron 03, a nigrosine-based dye; Bontron P-51, a quaternary ammonium salt; Bontron S-34, a metal-containing azo dye; E-82, an oxynaphthoic acid-based metal complex; E-84, a salicylic acid-based metal complex; E-89, a phenolic condensate (all manufactured by Orient Chemical Industry Co., Ltd.); TP-302 and TP-415, quaternary ammonium salt molybdenum complexes (both manufactured by Hodogaya Chemical Co., Ltd.); LRA-901; LR-147, a boron complex (both manufactured by Nippon Carlit Co., Ltd.); copper phthalocyanine; perylene; quinacridone; and azo pigments.
[0125] There are no particular restrictions on the content of the charge control agent, and it can be appropriately selected according to the purpose, but it is preferably 0.1 parts by mass or more and 10 parts by mass or less, and more preferably 0.2 parts by mass or more and 5 parts by mass or less, per 100 parts by mass of the resin particles. When the content of the charge control agent is 10 parts by mass or less per 100 parts by mass of the resin particles, it is possible to prevent the toner containing the resin particles from becoming excessively charged, maintain the effect of the main charge control agent, prevent an increase in electrostatic attraction force with the developing roller, and suppress a decrease in the fluidity of the developer and a decrease in image density. These charge control agents can be dissolved and dispersed after melting and kneading with the masterbatch and resin, or they can be added when directly dissolving and dispersing in an organic solvent, or they can be fixed to the surface of the resin particles after the resin particles have been manufactured.
[0126] <<Flow improver>> The aforementioned fluidity improver is not particularly limited as long as it can be surface-treated to increase its hydrophobicity and prevent deterioration of fluidity and electrostatic properties even under high humidity conditions. It can be appropriately selected according to the purpose, and examples include silane coupling agents, silylation agents, silane coupling agents having alkyl fluoride compounds, organic titanate coupling agents, aluminum coupling agents, silicone oil, or modified silicone oil. These may be used individually or in combination of two or more.
[0127] There are no particular restrictions on the content of the fluidity improver, and it can be appropriately selected depending on the purpose, but it is preferably 0.01 parts by mass or more and 5.00 parts by mass or less, and more preferably 0.10 parts by mass or more and 2.00 parts by mass or less, per 100 parts by mass of the resin particles.
[0128] <<Cleaning performance enhancer>> The aforementioned cleaning agent is intended to remove any residual developer from the photoreceptor or primary transfer medium after transfer. The cleaning agent is not particularly limited and can be appropriately selected depending on the purpose. Examples include fatty acid metal salts or polymer fine particles. These may be used individually or in combination of two or more.
[0129] Examples of the fatty acid metal salt include zinc stearate, calcium stearate, or stearic acid.
[0130] The polymer fine particles are preferably polymer fine particles produced by soap-free emulsion polymerization, and examples include polymethyl methacrylate fine particles or polystyrene fine particles.
[0131] There are no particular restrictions on the volume-average particle size of the polymer fine particles, and they can be appropriately selected depending on the purpose. However, a relatively narrow particle size distribution is preferred, and a volume-average particle size of 0.01 μm to 1 μm is preferred.
[0132] There are no particular restrictions on the content of the cleaning performance improving agent, and it can be appropriately selected depending on the purpose, but it is preferably 0.01 parts by mass or more and 5.00 parts by mass or less, and more preferably 0.10 parts by mass or more and 2.00 parts by mass or less, per 100 parts by mass of the resin particles.
[0133] <<Magnetic materials>> There are no particular limitations on the magnetic material, and it can be appropriately selected depending on the purpose. Examples include iron powder, magnetite, or ferrite. These may be used individually or in combination of two or more. Among these, a white magnetic material is preferred in terms of color.
[0134] There are no particular restrictions on the content of the magnetic material, and it can be appropriately selected depending on the purpose, but it is preferably 20 parts by mass or more and 200 parts by mass or less, and more preferably 40 parts by mass or more and 150 parts by mass or less, per 100 parts by mass of the resin particles.
[0135] <<<Modifying agent>>> The aforementioned shape-modifying agent is added to modify the shape of the resin particles. There are no particular restrictions on the modifying agent, and it can be appropriately selected depending on the purpose, but it is preferable that it contains a layered inorganic mineral in which at least a portion of the interlayer ions of the layered inorganic mineral are modified with organic ions.
[0136] There are no particular limitations on the layered inorganic mineral in which at least a portion of the interlayer ions are modified with organic ions, and it can be appropriately selected according to the purpose. For example, a layered inorganic mineral having a basic smectite crystal structure modified with organic cations can be used. Smectite clay minerals have negatively charged layers, and cations exist between the layers to compensate for this. Interlayer compounds can be formed by ion exchange of these cations or adsorption of polar molecules. In addition, metal ions can be introduced by substituting some of the divalent metals in the layered inorganic mineral with trivalent metals. However, since introducing metal anions increases hydrophilicity, layered inorganic compounds in which at least a portion of the metal anions are modified with organic anions are preferred.
[0137] The layered inorganic mineral, in which at least a portion of the interlayer ions of the aforementioned layered inorganic mineral are modified with organic ions, can be obtained by using an organic cation modifier or an organic anion modifier.
[0138] The organic cation modifier is not particularly limited as long as it can be modified by organic ions as described above, and examples include quaternary alkylammonium salts, phosphonium salts, or imidazolium salts. These may be used individually or in combination of two or more. Among these, quaternary alkylammonium salts are preferred as the organic cation modifier.
[0139] The quaternary alkylammonium is not particularly limited, and examples include trimethylstearylammonium, dimethylstearylbenzylammonium, or oleylbis(2-hydroxyethyl)methylammonium.
[0140] The organic anion modifier is not particularly limited as long as it can modify the target with organic ions as described above, and examples thereof include sulfates, sulfonates, carboxylates, or phosphates having a branched, unbranched, or cyclic alkyl (C1 to C44) group, a branched, unbranched, or cyclic alkenyl (C1 to C22) group, a branched, unbranched, or cyclic alkoxy (C8 to C32) group, a branched, unbranched, or cyclic hydroxyalkyl (C2 to C22) group, an ethylene oxide skeleton, or a propylene oxide skeleton. These may be used singly or in combination of two or more. Among these, the organic anion modifier is preferably a carboxylic acid having an ethylene oxide skeleton.
[0141] The deforming agent is preferably added in the <a) oil phase preparation step> described later when the resin particles are produced by the (method for producing resin particles) described later. By modifying at least part of the ions between the layers of the layered inorganic mineral with organic ions, the layered inorganic mineral has appropriate hydrophobicity, so that the oil phase containing the material of the resin particles has non-Newtonian viscosity and can deform the resin particles. At this time, the content of the deforming agent in the material of the resin particles is preferably 0.05% by mass to 10% by mass, and more preferably 0.05% by mass to 5% by mass, relative to the total amount of the material of the resin particles.
[0142] The layered inorganic mineral is not particularly limited and may be appropriately selected according to the purpose, and examples thereof include montmorillonite, bentonite, hectorite, attapulgite, sepiolite, or a mixture thereof. Among these, organically modified montmorillonite or organically modified bentonite is preferable, since the layered inorganic mineral obtained by modifying at least part of the interlayer ions of the layered inorganic mineral with organic ions does not affect the toner properties when the resin particles are used in a toner, allows easy viscosity adjustment, and can be added in a small amount.
[0143] Commercially available layered inorganic minerals in which at least a portion of the interlayer ions of the aforementioned layered inorganic mineral are modified with organic ions include, for example, quaternium-18 bentonite such as Bentone 3, Bentone 38, Bentone 38V (all manufactured by Rheox), Thixogel VP (manufactured by United Catalyst), Kraton 34, Kraton 40, Kraton XL (all manufactured by Southern Clay); stearalkonium bentonite such as Bentone 27 (manufactured by Rheox), Thixogel LG (manufactured by United Catalyst), Kraton AF, Kraton APA (all manufactured by Southern Clay); and quaternium-18 / benzalkonium bentonite such as Kraton HT, Kraton PS (both manufactured by Southern Clay). Among these, Kraton AF and Kraton APA are preferred.
[0144] Furthermore, as a layered inorganic mineral in which at least a portion of the interlayer ions of the aforementioned layered inorganic mineral are modified with organic ions, a more preferable option is one in which DHT-4A (registered trademark) (manufactured by Kyowa Chemical Industry Co., Ltd.) is modified with an organic anion modifier represented by the following general formula (I). An example of an organic anion modifier represented by the following general formula (I) is Hythenol (registered trademark) 330T (manufactured by Daiichi Kogyo Seiyaku Co., Ltd.).
[0145] R1(OR2) n OSO3M...General formula (I) (In the above general formula (I), R1 represents an alkyl group having 13 carbon atoms, R2 represents an alkylene group having 2 to 6 carbon atoms, n represents an integer from 2 to 10, and M represents a monovalent metallic element.)
[0146] <<Core-shell structure>> The resin particles may have a core-shell structure. In this specification, "having a core-shell structure" means a structure having a core layer and a shell layer, "shell layer" means a layer made of resin present in the outermost layer of the resin particle, and "core layer" means the region within the resin particle excluding the shell layer. The core layer and the shell layer are formed heterogeneously, not completely incompatible with each other. In the core-shell structure described above, it is preferable that the surface of the core layer is covered by the shell layer. In the core-shell structure described above, the surface of the core layer may or may not be completely covered by the shell layer. Examples of configurations in which the surface of the core layer is not completely covered by the shell layer include a configuration in which the core layer is covered by the shell layer in a mesh-like manner, and a configuration in which the core layer is partially exposed from the shell layer. Among these, from the viewpoint of filming resistance, it is preferable that the surface of the core layer is completely covered by the shell layer.
[0147] -Resin for shells- There are no particular restrictions on the shell resin constituting the shell layer, and it can be appropriately selected according to the purpose, but a resin that does not contain the crystalline resin is preferred, the amorphous resin is more preferred, and the amorphous polyester resin B is particularly preferred.
[0148] As mentioned above, the shell resin may be obtained by polycondensation of a polyhydric alcohol and a polyhydric carboxylic acid. The shell resin may contain the biomass-derived resin, or it may not contain the biomass-derived resin. From the viewpoint of filming resistance, it is preferable that the shell resin does not contain aliphatic hydrocarbons.
[0149] There are no particular limitations on the method for confirming that the shell layer does not contain the aliphatic hydrocarbons, and a suitable method can be selected depending on the purpose. For example, this can be confirmed by analyzing the surface (shell layer) composition using nano-IR (also referred to as "AMF-IR"). By using an analytical technique that combines nano-IR atomic force microscopy (AFM) with IR to achieve nanoscale resolution, the compositional structure can be determined by obtaining the IR spectrum of the surface layer (shell layer) of the resin particles. Specifically, the resin particles are embedded in epoxy resin (S-31, manufactured by DEVCON) and cured. A cross-section is then made using a knife, and the resin particles are cut to a thickness of 60 nm using an ultrasonic ultramicrotome (Leica EM UC7, manufactured by Leica) to produce ultrathin sections of the resin particles. The prepared ultrathin sections of toner are collected on a substrate (ZnS), and the measurement area (shell layer) is measured using AFM-IR method with a nanoscale infrared spectroscopy system (e.g., nanoIR2, manufactured by Anasys Instruments). The measurement range is 1,900 cm². -1 From 910cm -1 The resolution is 2cm. -1 Therefore, the chemical structure of the measurement site (shell layer) can be analyzed from the obtained AFM-IR absorption spectrum. Thus, this analysis can identify whether aliphatic hydrocarbons are present in the surface layer (shell layer). Furthermore, by designating the measurement location as the core layer, the chemical structure of the core layer can also be analyzed.
[0150] There are no particular restrictions on the average thickness of the shell layer, and it can be appropriately selected depending on the purpose, but 50 nm to 500 nm is preferred, and 100 nm to 200 nm is more preferred. If the average thickness of the shell layer is 50 nm or more, the core layer inside the resin particles can be protected and the mechanical strength can be improved, and if it is 500 nm or less, sufficient mechanical strength can be maintained without hindering low-temperature fixation. In this specification, "average shell layer thickness" refers to the average thickness obtained by selecting 50 resin particles with a weight-average particle size within ±2.0 μm, measuring the thickness of the shell layer of each particle using the method described below, and averaging the thicknesses of the shell layers of these 50 resin particles.
[0151] There are no particular restrictions on the coverage rate of the shell layer on the surface of the core layer, and it can be appropriately selected depending on the purpose, but 50% to 100% is preferred, and 80% to 100% is more preferred. A coverage rate of 100% means that the entire surface area of the core layer in the resin particles is covered with the shell layer. The coverage rate (%) of the core layer surface by the shell layer can be calculated by the following formula (3). Coverage rate (%) = (Area of covered region) / (Total surface area of resin particles) × 100 ... Equation (3) In formula (3) above, "total surface area of resin particles" means the sum of the area of the covered region and the exposed core layer area, "area of the covered region" means the area of the total surface area of resin particles in which the core layer is covered by the shell layer, and "exposed core layer area" means the area of the total surface area of resin particles in which the core layer is not covered by the shell layer.
[0152] There are no particular limitations on the method for confirming that the resin particles have a core-shell structure, and a suitable method can be selected depending on the purpose. For example, the resin particles may be embedded in epoxy resin (S-31, manufactured by DEVCON) and cured, then cross-sectioned with a knife, and excised to a thickness of 60 nm using an ultrasonic ultramicrotome (Leica EM UC7, manufactured by Leica) to prepare ultrathin sections of the resin particles. The prepared ultrathin sections of the toner are then exposed to gas with ruthenium tetroxide (RuO4) to distinguish and stain the shell and core. The gas exposure time can be adjusted as appropriate depending on the contrast during observation. Subsequently, the structure can be confirmed by observing a cross-sectional image of the resin particles using a transmission electron microscope (H-7500, manufactured by Hitachi High-Tech Corporation) at an accelerating voltage of 120 kV.
[0153] Furthermore, in the TEM images observed using the method described above, the core layer coverage area on the surface of the resin particle (the area in the resin particle where the core layer is covered by the shell layer) and the exposed core layer area (the area in the resin particle where the core layer is not covered by the shell layer) can be distinguished by the difference in brightness values. Therefore, by performing binarization processing on the TEM images observed using the method described above using image processing software, the shell layer can be identified by its contrast ratio, and the thickness of the shell layer can be measured.
[0154] Image-J can be used as the image processing software. The method for calculating the average thickness of the shell layer using Image-J is as follows. (1) Use Straight Line to draw a straight line that traces the scale. Use Analyze's Set Scale to set its actual length and units. (2) The outer circumference of a single resin particle in the cross-sectional image of the resin particle is enclosed by freehand sections to create "region 1". (3) The outer periphery of the region excluding the shell layer in the cross-sectional image of one resin particle (i.e., the boundary between the shell layer and the core layer) is enclosed with freehand sections to create "region 2". (4) Determine the center of mass of "region 1" using Analyze. (5) Using a proprietary plugin, a straight line is drawn from the outer perimeter of "region 1," that is, from the coordinates obtained by dividing the line that encloses the outer perimeter of one resin particle in (2) with Freehand-sections into 100 equally spaced sections, toward the center of gravity of the resin particle determined in (4). (6) The length obtained by subtracting the length passing through "Region 2" from the length of each of the 100 straight lines created in (5) above is calculated using the straight lines that trace the scale created in (1) above, and the average of the 100 values is taken as the thickness of the shell layer of one resin particle. (7) Perform the operations described in (2) to (6) above for 50 resin particles and calculate the average thickness of the shell layer of the 50 resin particles. This average value is taken as the average thickness of the shell layer in the present invention.
[0155] Furthermore, the method for calculating the coverage rate of the shell layer using Image-J is as follows. (1) Trace the portion of the outer periphery of a single resin particle covered by the shell layer in the cross-sectional image of the resin particle using Freehand Line, and measure the length of the traced line using Analyze. This length is defined as "Length 1". (2) Trace the outer circumference of one resin particle in the cross-sectional image of the resin particle using Freehand Line, and measure the length of the traced line using Analyze. This length shall be "Length 2". (3) Calculate length 1 / length 2 × 100 and use this as the coverage rate of the shell layer of one resin particle. (4) Perform the operations described in (1) to (3) above for 50 resin particles and calculate the average value of the shell layer coverage rate for the 50 resin particles. This average value is taken as the shell layer coverage rate in the present invention.
[0156] <Volume-average particle size> There are no particular restrictions on the volume-average particle size (D4) of the resin particles, and it can be appropriately selected depending on the purpose, but it is preferably 3 μm or more and 7 μm or less. Furthermore, there are no particular restrictions on the ratio (D4 / Dn) of the volume-average particle size (D4) of the resin particles to the number-average particle size (Dn) of the resin particles, and it can be appropriately selected depending on the purpose, but it is preferably 1.2 or less. Furthermore, it is preferable that the resin particles contain at least 1% to 10% of a component having a volume-average particle size of 2 μm or less.
[0157] The volume-average particle size (D4), number-average particle size (Dn), and their ratio (D4 / Dn) of the aforementioned resin particles can be measured using, for example, a Coulter Counter TA-II or a Coulter Multisizer II (both manufactured by Coulter). In this specification, the values obtained using the Coulter Multisizer II will be used. The measurement method is described below.
[0158] First, a mixture is obtained by adding 0.1 mL to 5 mL of a surfactant (preferably polyoxyethylene alkyl ether (a nonionic surfactant)) as a dispersant to 100 mL to 150 mL of an electrolytic aqueous solution. To this mixture, 2 mg to 20 mg of the sample to be measured is added. The electrolytic aqueous solution in which the sample to be measured is suspended is subjected to dispersion treatment in an ultrasonic disperser for about 1 to 3 minutes. The volume and number of the resin particles are measured using the measuring device (Coulter Multisizer II) with a 100 μm aperture, and the volume distribution and number distribution are calculated. From the obtained distribution, the volume-average particle size (D4) and number-average particle size (Dn) of the resin particles can be determined. The electrolytic aqueous solution mentioned above is prepared by using primary sodium chloride to create a 1% by mass sodium hydrochloride aqueous solution. For example, ISOTON-II (manufactured by Coulter) can be used.
[0159] The 13 channels used are 2.00 μm to less than 2.52 μm, 2.52 μm to less than 3.17 μm, 3.17 μm to less than 4.00 μm, 4.00 μm to less than 5.04 μm, 5.04 μm to less than 6.35 μm, 6.35 μm to less than 8.00 μm, 8.00 μm to less than 10.08 μm, 10.08 μm to less than 12.70 μm, 12.70 μm to less than 16.00 μm, 16.00 μm to less than 20.20 μm, 20.20 μm to less than 25.40 μm, 25.40 μm to less than 32.00 μm, and 32.00 μm to less than 40.30 μm, targeting particles with a particle size of 2.00 μm to less than 40.30 μm.
[0160] <Glass transition temperature (Tg) and melting point (Tm)> <<Method for measuring glass transition temperature (Tg) and melting point (Tm)>> The glass transition temperature (Tg) and melting point (Tm) as used herein can be measured, for example, using a DSC system (differential scanning calorimeter) ("Q-200", manufactured by TA Instruments). Specifically, the glass transition temperature (Tg) and melting point (Tm) of the target sample can be measured by the following procedure. First, approximately 5.0 mg of the target sample is placed in an aluminum sample container, the sample container is placed on a holder unit, and set in an electric furnace. Next, under a nitrogen atmosphere, the sample is heated from -80°C to 150°C at a temperature elevation rate of 10°C / min (first temperature elevation). Thereafter, the sample is cooled from 150°C to -80°C at a temperature lowering rate of 10°C / min, and further heated to 150°C at a temperature elevation rate of 10°C / min (second temperature elevation). In each of the first temperature elevation and the second temperature elevation, a DSC curve is measured using a differential scanning calorimeter ("Q-200", manufactured by TA Instruments).
[0161] From the obtained DSC curves, using the analysis program in the Q-200 system, the DSC curve at the first temperature elevation can be selected, and the glass transition temperature of the target sample at the first temperature elevation can be determined. Similarly, the DSC curve at the second temperature elevation can be selected, and the glass transition temperature of the target sample at the second temperature elevation can be determined.
[0162] In addition, from the obtained DSC curves, using the analysis program in the Q-200 system, the DSC curve at the first temperature elevation can be selected, and the endothermic peak top temperature of the target sample at the first temperature elevation can be determined as the melting point. Similarly, the DSC curve at the second temperature elevation can be selected, and the endothermic peak top temperature of the target sample at the second temperature elevation can be determined as the melting point.
[0163] In the present specification, when the resin particles described above are used as the target sample, the glass transition temperature at the first temperature elevation is denoted as [Tg1st], and the glass transition temperature at the second temperature elevation is denoted as [Tg2nd]. Further, in the present specification, regarding the glass transition temperature and melting point of the amorphous polyester resin A, the amorphous polyester resin B, the crystalline polyester resin C, and other constituent components such as the release agent, unless otherwise specified, the endothermic peak top temperature at the second temperature elevation is taken as the melting point of each target sample, and the Tg at the second temperature elevation is taken as the Tg of each target sample.
[0164] <<Tg1st (Resin Particles)>> There are no particular restrictions on the glass transition temperature [Tg1st(resin particles)] during the first heating step of differential scanning calorimetry (DSC) of the resin particles, and it can be appropriately selected according to the purpose. However, from the viewpoint of low-temperature fixability, it is preferably 20°C to 50°C, and more preferably 35°C to 45°C. If the [Tg1st(resin particles)] is 20°C or higher, a decrease in heat resistance for storage, blocking in the developing machine, and filming on the photoreceptor can be suppressed. If the [Tg1st(resin particles)] is 50°C or lower, a decrease in the low-temperature fixability of the resin particles can be suppressed.
[0165] Conventionally, when the glass transition temperature (Tg) of toner is around 50°C or below, toner aggregation is more likely to occur due to temperature changes during transportation and storage, especially in summer or tropical regions. As a result, solidification occurs in the toner bottle and toner adheres to the developing machine. Furthermore, toner clogging in the toner bottle can lead to poor replenishment, and toner adherence to the developing machine can easily cause image abnormalities.
[0166] Even if the toner containing the aforementioned resin particles has a lower glass transition temperature (Tg) than conventional toners, if the amorphous polyester resin A, which is the low Tg component in the toner, is nonlinear, the toner can maintain its heat resistance for storage. In particular, if the amorphous polyester resin A has urethane bonds or urea bonds with high cohesive force, the effect of maintaining heat resistance for storage becomes even more pronounced.
[0167] <<[Tg2nd (resin particles)]>> There are no particular restrictions on the glass transition temperature [Tg2nd(resin particles)] during the second heating step of differential scanning calorimetry (DSC) of the resin particles, and it can be appropriately selected according to the purpose, but it is preferably 0°C to 30°C, and more preferably 0°C to 15°C. If the [Tg2nd(resin particles)] is 0°C or higher, it is possible to suppress a decrease in the blocking resistance of the fixed image (printed material), and if it is 30°C or lower, it is possible to suppress a decrease in low-temperature fixability and glossiness. The value of the aforementioned [Tg2nd (resin particles)] can be adjusted by, for example, the Tg of the crystalline polyester resin and the blending amount thereof.
[0168] <<Difference [[Tg1st (resin particles)] - [Tg2nd (resin particles)]]>> The difference [[Tg1st (resin particles)] - [Tg2nd (resin particles)]] between the glass transition temperature in the first temperature rise [Tg1st (resin particles)] and the glass transition temperature in the second temperature rise [Tg2nd (resin particles)] in differential scanning calorimetry (DSC) of the resin particles is not particularly limited and may be appropriately selected according to the purpose, but is preferably 10°C or higher. The upper limit of the difference [[Tg1st (resin particles)] - [Tg2nd (resin particles)]] is not particularly limited and may be appropriately selected according to the purpose, but is preferably 50°C or lower. When the difference [[Tg1st (resin particles)] - [Tg2nd (resin particles)]] is 10°C or higher, it is advantageous in that the low-temperature fixability is more excellent. Further, that the difference [[Tg1st (resin particles)] - [Tg2nd (resin particles)]] is 10°C or higher means that the crystalline polyester resin C, which was present in an incompatible state before heating (before the first temperature rise), and the amorphous polyester resin A and the amorphous polyester resin B enter a compatible state after heating (after the first temperature rise). The compatible state after heating does not need to be a completely compatible state.
[0169] <<Tg2nd (THF-insoluble matter)>> The glass transition temperature [Tg2nd (THF-insoluble matter)] in the second temperature rise in differential scanning calorimetry (DSC) of the tetrahydrofuran (THF)-insoluble matter of the resin particles is not particularly limited and may be appropriately selected according to the purpose, but is preferably -40°C or higher and 30°C or lower, and more preferably 0°C or higher and 20°C or lower. When the [Tg2nd (THF-insoluble matter)] is -40°C or higher, the advantage that the decrease in blocking resistance of a fixed image (printed matter) can be suppressed is obtained, and when it is 30°C or lower, the advantage that the decrease in low-temperature fixability and glossiness can be suppressed is obtained.
[0170] The aforementioned [Tg2nd (THF-insoluble content)] can be adjusted, for example, by changing the number of carbon atoms in the polyhydric alcohol and polyhydric carboxylic acid of amorphous polyester resin A.
[0171] <<Melting point (Tm)>> There are no particular restrictions on the melting point (Tm) of the resin particles, and it can be appropriately selected depending on the purpose, but it is preferably 60°C or higher and 80°C or lower.
[0172] <Storage modulus> <<Method for measuring the storage modulus G'>> The storage modulus (G') under various conditions can be measured, for example, using a dynamic viscoelasticity measuring device (ARES, manufactured by TA Instruments). The measurement frequency is 1 Hz. Specifically, the sample to be measured is molded into a pellet with a diameter of 8 mm and a thickness of 1 mm to 2 mm, fixed to an 8 mm diameter parallel plate, stabilized at 40°C, and then heated to 200°C at a heating rate of 2.0°C / min with a frequency of 1 Hz (6.28 rad / s) and a strain of 0.1% (strain control mode), and the storage modulus is measured. In this specification, the storage modulus at 40°C is sometimes represented as [G'(40)], and the storage modulus at 100°C is sometimes represented as [G'(100)].
[0173] <<[G'(100)(THF-insoluble)], and [[G'(40)(THF-insoluble)] / [G'(100)(THF-insoluble)]]>> There are no particular restrictions on the storage modulus at 100°C of the tetrahydrofuran (THF)-insoluble portion of the resin particles [G'(100)(THF-insoluble portion)], and it can be appropriately selected depending on the purpose, but 1.0 × 10 5 Pa~1.0×10 7 Pa is preferred, 5.0 × 10 5 Pa~5.0×10 6 Pa is more preferable. When the storage modulus [G'(100)(THF-insoluble)] is within the more preferable range, it is advantageous in that it provides better low-temperature fixation.
[0174] The ratio of the storage elastic modulus at 40°C [G'(40) (THF-insoluble content)] to the storage elastic modulus at 100°C [G'(100) (THF-insoluble content)] ([G'(40) (THF-insoluble content)] / [G'(100) (THF-insoluble content)]) of the THF-insoluble content of the resin particles is not particularly limited and can be appropriately selected according to the purpose, but it is preferably 3.5×10 or less. When the ratio [G'(40) (THF-insoluble content)] / [G'(100) (THF-insoluble content)] is 3.5×10 or less, deterioration of low-temperature fixability can be suppressed.
[0175] Further, in the resin particles, when the [G'(100) (THF-insoluble content)] is 1.0×10 5 Pa to 1.0×10 7 Pa, and the ratio [G'(40) (THF-insoluble content)] / [G'(100) (THF-insoluble content)] is 3.5×10 or less, it is advantageous in that it promotes compatibilization between the crystalline resin and the amorphous polyester resin which is a high Tg component, lowers the 1 / 2 outflow temperature measured by a thermal flow evaluation apparatus (flow tester), and improves image gloss.
[0176] The values of [G'(100) (THF-insoluble content)] and [G'(40) (THF-insoluble content)] can be adjusted by, for example, the resin composition (a di- or higher-functional polyhydric alcohol and a di- or higher-functional acid component). Specifically, the adjustment can be performed, for example, in the following manner. To increase the storage elastic modulus [G'], it can be adjusted by shortening the distance of ester bonds in the resin, or adopting a resin composition having an aromatic ring. To decrease the storage elastic modulus [G'], it can be adjusted by using a linear polyester resin, or using a polyhydric alcohol having an alkyl group in the side chain as a constituent component of the polyester resin.
[0177] <<THF-insoluble content>> The THF-insoluble content of the resin particles can be obtained as follows. One part resin particles are added to 100 parts tetrahydrofuran (THF) and refluxed for 6 hours. The insoluble components are then separated from the supernatant by centrifugation to allow them to settle. The mass of the insoluble components dried at 40°C for 20 hours is divided by the mass of the resin particles used initially, and this result is multiplied by 100 to calculate the THF insoluble content.
[0178] There are no particular restrictions on the content of THF-insoluble matter in the resin particles, and it can be appropriately selected depending on the purpose, but it is preferably 20% by mass or more, more preferably 30% by mass or more, and even more preferably 40% by mass or more. The higher the content of THF-insoluble matter, the more crosslinking components are present in the resin particles, and when the THF-insoluble matter is 20% by mass or more, the filming resistance is improved.
[0179] <<Measuring Molecular Weight>> The molecular weight of each component of the aforementioned resin particles can be measured, for example, under the following analytical conditions. [Analysis conditions] • Gel permeation chromatography (GPC) measuring device: GPC-8220GPC (manufactured by Tosoh Corporation) Column: TSKgel® SuperHZM-H 15cm 3-row (manufactured by Tosoh Corporation) ·Temperature: 40℃ • Detector: RI (refractive index) detector • Solvent: Tetrahydrofuran (THF) or chloroform Flow rate: 0.35 mL / min • Sample: Inject 100 μL of 0.15 mass% of the sample. • Sample pretreatment: The resin particles are dissolved in tetrahydrofuran THF (containing stabilizer, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) or chloroform at a concentration of 0.15% by mass, then filtered through a 0.2 μm filter, and the filtrate is used as the sample. 100 μL of the sample solution is injected and measured.
[0180] For molecular weight measurement of a sample, the molecular weight distribution of the sample is calculated from the relationship between the logarithm of a calibration curve prepared using several monodisperse polystyrene standard samples and the count. Examples of standard polystyrene samples used for calibration curve preparation include Showdex® STANDARD (manufactured by Showa Denko K.K.) Std. No. S-6550, S-1700, S-740, S-321, S-129, S-10, S-2.9, and S-0.6.
[0181] <Methods for calculating and analyzing various properties of the constituent components of resin particles> The glass transition temperature (Tg), melting point, acid value, hydroxyl value, and molecular weight of the amorphous polyester resin A, amorphous polyester resin B, crystalline polyester resin C, and mold release agent in the resin particles, as well as the mass ratio of each component in the resin particles, may be measured individually, or they may be calculated by separating them from the actual resin particles using gel permeation chromatography (GPC) or the like, and then analyzing each separated component using the analytical methods described later.
[0182] The separation of each component in the resin particles by GPC can be carried out, for example, by the following method. In GPC measurements using chloroform as the mobile phase, the eluate is separated using a fraction collector or similar device, and the fraction corresponding to the desired molecular weight portion of the total integral of the elution curve is collected.
[0183] After concentrating and drying this collected eluate using an evaporator or the like, the solid components are dissolved in a deuterated solvent such as deuterated chloroform or deuterated THF. 1 ¹H-NMR measurements are performed, and the ratio of each component of the resin particles in the eluted components is calculated from the integral ratio of each element.
[0184] Another method involves concentrating the collected eluate, hydrolyzing it with sodium hydroxide or the like, and then qualitatively and quantitatively analyzing the decomposition products using high-performance liquid chromatography (HPLC) or the like to calculate the ratio of each component of the resin particles.
[0185] Furthermore, if the method for producing the resin particles involves generating the amorphous polyester resin A through an extension reaction and / or crosslinking reaction between the nonlinear reactive precursor and the curing agent, thereby forming the matrix particles of the resin particles, the actual resin particles may be separated by GPC or the like to determine the glass transition temperature (Tg) of the amorphous polyester resin A. Alternatively, the amorphous polyester resin A may be synthesized separately through an extension reaction and / or crosslinking reaction between the nonlinear reactive precursor and the curing agent, and the glass transition temperature (Tg) and other properties may be measured from the synthesized amorphous polyester resin A.
[0186] <<Means for separating resin particle components>> An example of a means for separating each component when analyzing the aforementioned resin particles is shown in detail. First, 1 g of the resin particles is placed in 100 mL of chloroform and stirred at 25°C for 30 minutes to obtain a solution in which the soluble components have dissolved. This solution is filtered through a membrane filter with a mesh size of 0.2 μm to obtain the chloroform-soluble components in the resin particles. Next, this is dissolved in chloroform to prepare a sample for GPC measurement and injected into the GPC used for molecular weight measurement of each resin as described above.
[0187] On the other hand, a fraction collector is placed at the eluate outlet of the GPC, and the eluate is collected at predetermined count intervals, obtaining eluate at intervals of 5% area percentage from the start of elution (rise of the curve) on the elution curve. Next, for each eluate, 30 mg of the sample is dissolved in 1 mL of deuterated chloroform, and 0.05 volume% of tetramethylsilane (TMS) is added as a reference substance. The obtained solution is packed into a 5 mm diameter glass tube for nuclear magnetic resonance (NMR) spectroscopy, and a nuclear magnetic resonance spectrometer (e.g., JNM-AL400, manufactured by JEOL Ltd.) is used to perform 128 integrations at a temperature of 23°C to 25°C to obtain a spectrum. From the peak integration ratio of the obtained spectrum, the monomer composition and constituent ratio of amorphous polyester resin A, amorphous polyester resin B, and crystalline polyester resin C contained in the resin particles can be determined.
[0188] For example, peak assignment can be performed as follows, and the component ratios of the constituent monomers can be determined from their respective integral ratios. Peak assignment can be done, for example, as follows. • Around 8.25 ppm: Derived from the benzene ring of trimellitic acid (one hydrogen atom) • Around 8.07 ppm to 8.10 ppm: Derived from the benzene ring of terephthalic acid (4 hydrogen atoms) • Around 7.1 ppm to 7.25 ppm: Derived from the benzene ring of bisphenol A (4 hydrogen atoms) • Around 6.8 ppm: Derived from the benzene ring of bisphenol A (4 hydrogen atoms) and the double bond of fumaric acid (2 hydrogen atoms). • Approximately 5.2 ppm to 5.4 ppm: Derived from methine (equivalent to one hydrogen atom) in the bisphenol A propylene oxide adduct. • Around 3.7 ppm to 4.7 ppm: Methylene-derived from bisphenol A propylene oxide adduct (2 hydrogen atoms) and methylene-derived from bisphenol A ethylene oxide adduct (4 hydrogen atoms) • Around 1.6 ppm: Derived from the methyl group of bisphenol A (equivalent to 6 hydrogen atoms)
[0189] From these results, for example, the eluate recovered in a fraction containing 90% or more by mass of amorphous polyester resin A can be treated as amorphous polyester resin A. Similarly, the eluate recovered in a fraction containing 90% or more by mass of amorphous polyester resin B can be treated as amorphous polyester resin B. Furthermore, the eluate recovered in a fraction containing 90% or more by mass of crystalline polyester resin C can be treated as crystalline polyester resin C.
[0190] The method for producing the resin particles is such that the proportion of the crystalline resin in the region within 150 nm from the outermost surface of the resin particles is 4% or less of the total amount of the toner resin particles, and radioactive carbon isotopes 14There is no particular limitation as long as the C concentration can be 5.4 pMC or higher, and it can be appropriately selected according to the purpose. Examples thereof include known emulsion aggregation methods, but production by the method for producing resin particles of the present invention described later is preferred.
[0191] (Method for Producing Resin Particles) The method for producing resin particles of the present invention includes: a) a step of preparing an oil phase in which at least a crystalline resin and an amorphous polyester resin are dissolved or dispersed in an organic solvent (hereinafter sometimes referred to as "oil phase preparation step"); b) a step of adding an aqueous medium to the oil phase to cause phase inversion from a water-in-oil dispersion to an oil-in-water dispersion (hereinafter sometimes referred to as "phase inversion emulsification step"); and c) a step of aggregating particles of the oil-in-water dispersion to obtain aggregated particles, then adding an amorphous polyester resin to obtain resin particles (hereinafter sometimes referred to as "aggregation step"), and optionally further includes other steps such as an aqueous phase preparation step, a solvent removal step, a fusing step, a washing step, a drying step, a classification step, and an annealing step. The alcohol monomer of the amorphous polyester resin contains propylene glycol, and the abundance ratio of the crystalline resin in a region within 150 nm from the outermost surface of the resin particles is 4% or less relative to the total amount of the resin particles, and the radioactive carbon isotope of the resin particles 14 The C concentration is 5.4 pMC or higher.
[0192] <a) Oil Phase Preparation Step> The oil phase preparation step is a step of preparing an oil phase in which at least a crystalline resin and an amorphous polyester resin are dissolved or dispersed in an organic solvent. The crystalline resin is as described in the section <<Crystalline Resin>> under (Resin Particles and Resin Particles for Toner). The amorphous polyester resin is as described in the section "Amorphous Polyester Resin" of the above (Resin Particles and Toner Resin Particles), and the oil phase may contain amorphous polyester resin A and amorphous polyester resin B, and may also contain the nonlinear reactive precursor, amorphous polyester resin B and the curing agent. The curing agent may be contained in an aqueous medium as described later. The oil phase may further contain a coloring agent and a mold release agent, if necessary. The aforementioned colorants and release agents are as described in the sections "Colorants" and "Release Agents" under "Other Components" in (Resin Particles and Toner Resin Particles) above.
[0193] There are no particular restrictions on the organic solvent, and it can be appropriately selected depending on the purpose, but an organic solvent with a boiling point of less than 150°C is preferred because it is easy to remove. The organic solvent with a boiling point of less than 150°C is not particularly limited and can be appropriately selected depending on the purpose. Examples include toluene, xylene, benzene, carbon tetrachloride, methylene chloride, 1,2-dichloroethane, 1,1,2-trichloroethane, trichloroethylene, chloroform, monochlorobenzene, dichloroethylidene, methyl acetate, ethyl acetate, methyl ethyl ketone, or methyl isobutyl ketone. These may be used individually or in combination of two or more. Among these, ethyl acetate, toluene, xylene, benzene, methylene chloride, 1,2-dichloroethane, chloroform, or carbon tetrachloride are preferred as the organic solvent, with ethyl acetate being more preferred.
[0194] There are no particular restrictions on the amount of the organic solvent used, and it can be appropriately selected depending on the purpose, but preferably 40 to 300 parts by mass, more preferably 60 to 140 parts by mass, and even more preferably 80 to 120 parts by mass per 100 parts by mass of the raw material for the resin particles.
[0195] There are no particular restrictions on the method for preparing the oil phase, and it can be appropriately selected depending on the purpose. For example, one method is to gradually add the materials for the oil phase to the organic solvent while stirring, and dissolve or disperse them. For the aforementioned dispersion, known methods can be used, such as dispersers like bead mills or disc mills.
[0196] There are no particular restrictions on the particle size of the dispersed crystalline resin in the oil phase, and it can be appropriately selected depending on the purpose, but it is preferably 20 nm to 500 nm, and more preferably 50 nm to 360 nm. In this specification, the dispersed particle size of the crystalline resin is the volume-average particle size.
[0197] The dispersed particle size of the crystalline resin can be measured, for example, using a nanotrack particle size distribution analyzer (UPA-EX150, Nikkiso Co., Ltd., dynamic light scattering method / laser Doppler method). The specific measurement method involves adjusting the dispersion of the crystalline resin to the measurement concentration range and then performing the measurement. Prior to this, a background measurement is performed using only the dispersion solvent of the dispersion. This method allows for measurements from several tens of nanometers to several micrometers.
[0198] <Aqueous phase (aqueous medium) production process> The aforementioned aqueous phase preparation step is a step in which an aqueous phase (aqueous medium) is prepared. The aqueous medium is not particularly limited and can be appropriately selected depending on the purpose. Examples include water, a solvent miscible with water, or a mixture thereof. These may be used individually or in combination of two or more. Among these, water is preferred.
[0199] Examples of the aforementioned water include ion-exchanged water.
[0200] Examples of solvents that can be miscible with water include organic solvents. The organic solvent is not particularly limited as long as it is miscible with water, and can be appropriately selected according to the purpose. Examples thereof include ester-based solvents such as methyl acetate, ethyl acetate, and butyl acetate; ketone-based solvents such as acetone, methyl ethyl ketone, and methyl isobutyl ketone; alcohol-based solvents such as methanol, isopropanol, and ethylene glycol; amide-based solvents such as dimethylformamide; ether-based solvents such as tetrahydrofuran; and cellosolve-based solvents. The concentration of the organic solvent in the aqueous medium is not particularly limited, but is preferably not higher than the saturation concentration relative to ion-exchanged water from the viewpoint of granulation properties.
[0201] <b) Phase inversion emulsification step> The phase inversion emulsification step is a step of adding an aqueous medium to the oil phase to cause phase inversion from a water-in-oil dispersion to an oil-in-water dispersion. Thereby, a fine particle dispersion (oil droplets) is obtained. Further, when the oil phase contains the non-linear reactive precursor, the amorphous polyester resin A may be produced by subjecting the curing agent and the non-linear reactive precursor to an elongation reaction and / or a crosslinking reaction in the phase inversion emulsification step. The amorphous polyester resin A is as described in the section of <<<Amorphous Polyester Resin A>>> for the (resin particles and toner resin particles).
[0202] When the amorphous polyester resin A is produced in the phase inversion emulsification step, specifically, the amorphous polyester resin A can be produced, for example, by any one of the following methods (1) to (3). (1) A method of emulsifying or dispersing an oil phase containing the non-linear reactive precursor and the curing agent in the aqueous medium, and subjecting the curing agent and the non-linear reactive precursor to an elongation reaction and / or a crosslinking reaction in the aqueous medium to produce the amorphous polyester resin A. (2) A method of producing the amorphous polyester resin A by emulsifying or dispersing the oil phase containing the non-linear reactive precursor in an aqueous medium to which the curing agent has been added in advance, and subjecting the curing agent and the non-linear reactive precursor to an elongation reaction and / or a crosslinking reaction in the aqueous medium. (3) A method of producing the amorphous polyester resin A by emulsifying or dispersing the oil phase containing the non-linear reactive precursor in an aqueous medium, then adding the curing agent into the aqueous medium, and subjecting the curing agent and the non-linear reactive precursor to an elongation reaction and / or a crosslinking reaction from the particle interface in the aqueous medium.
[0203] Note that when the curing agent and the non-linear reactive precursor are subjected to an elongation reaction and / or a crosslinking reaction from the interface of the resin particles, the amorphous polyester resin A is preferentially formed on the surface of the generated resin particles, and a concentration gradient of the amorphous polyester resin A can also be provided in the resin particles.
[0204] The reaction conditions (reaction time, reaction temperature) for producing the amorphous polyester resin A are not particularly limited, and can be appropriately selected according to the combination of the curing agent and the non-linear reactive precursor. The reaction time is not particularly limited and can be appropriately selected according to the purpose, and is preferably 10 minutes or more and 40 hours or less, more preferably 2 hours or more and 24 hours or less. The reaction temperature is not particularly limited and can be appropriately selected according to the purpose, and is preferably 0°C or higher and 150°C or lower, more preferably 40°C or higher and 98°C or lower.
[0205] The method for performing phase inversion emulsification on the dispersion containing the non-linear reactive precursor in the aqueous medium is not particularly limited and can be appropriately selected according to the purpose. Examples thereof include a method of obtaining a fine particle dispersion by phase inversion emulsification, in which the oil phase is neutralized with a base or the like, then the aqueous phase is added thereto, and the water-in-oil dispersion is phase-inverted to an oil-in-water dispersion.
[0206] Either a basic inorganic compound or a basic organic compound may be used as the base for neutralizing the oil phase. The basic inorganic compound is not particularly limited and can be appropriately selected depending on the purpose. Examples include sodium hydroxide, potassium hydroxide, lithium hydroxide, ammonia, sodium carbonate, sodium bicarbonate, potassium carbonate, potassium bicarbonate, and ammonia. The basic organic compound is not particularly limited and can be appropriately selected depending on the purpose. Examples include N,N-dimethylethanolamine, N,N-diethylethanolamine, triethanolamine, trippropanolamine, tributanolamine, triethylamine, n-propylamine, n-butylamine, isopropylamine, monomethanolamine, morpholine, methoxypropylamine, pyridine, vinylpyridine, and isophoronediamine.
[0207] The neutralization of the oil phase can be carried out by uniformly mixing or dispersing it using a conventional stirrer or dispersion device. The dispersion device is not particularly limited and examples include ultrasonic dispersers, bead mills, ball mills, roll mills, homomixers, ultramixers, disper mixers, through-type high-pressure dispersion devices, impact-type high-pressure dispersion devices, porous high-pressure dispersion devices, ultra-high-pressure homogenizers, and ultrasonic homogenizers. Conventional stirrers and dispersion devices may be used in combination.
[0208] There are no particular restrictions on the amount of the aqueous medium used when emulsifying the oil phase containing the resin particle material, and it can be appropriately selected according to the purpose. Preferably, the amount is 50 parts by mass or more and 2,000 parts by mass or less, and more preferably 100 parts by mass or more and 1,000 parts by mass or less, per 100 parts by mass of the resin particle material. If the amount of the aqueous medium used is 50 parts by mass or more per 100 parts by mass of the resin particle material, it is possible to prevent the dispersion state of the resin particle material from deteriorating and to suppress the failure to obtain resin particles of a predetermined particle size. Furthermore, if the amount of the aqueous medium used is 2,000 parts by mass or less per 100 parts by mass of the resin particle material, it is possible to suppress the increase in production costs.
[0209] When inverting and emulsifying the oil phase containing the aforementioned resin particle material, it is preferable to use a dispersant from the viewpoint of stabilizing dispersions such as oil droplets, giving them a desired shape, and sharpening the particle size distribution. There are no particular restrictions on the dispersant, and it can be appropriately selected depending on the purpose. Examples include surfactants, poorly water-soluble inorganic compound dispersants, or polymer-based protective colloids. These may be used individually or in combination of two or more. Among these, surfactants are preferred as the dispersant.
[0210] The surfactant is not particularly limited and can be appropriately selected depending on the purpose. Examples include anionic surfactants, cationic surfactants, nonionic surfactants, or amphoteric surfactants.
[0211] The anionic surfactant is not particularly limited and can be appropriately selected depending on the purpose. Examples include alkylbenzene sulfonates, α-olefin sulfonates, or phosphate esters. Among these, the anionic surfactant having a fluoroalkyl group is preferred.
[0212] A catalyst can be used in the extension reaction and / or crosslinking reaction when producing the amorphous polyester resin A. The catalyst is not particularly limited and can be appropriately selected depending on the purpose. Examples include dibutylsulfurate and dioctylsulfurate.
[0213] The aforementioned phase inversion emulsification can be carried out using a stirring blade. The aforementioned stirring blades are not particularly limited and can be appropriately selected depending on the viscosity of the solution. Examples include anchor blades, turbine blades, Faudler blades, full-zone blades, maxblend blades, or crescent blades.
[0214] The peripheral speed when using the stirring blade is not particularly limited and can be appropriately selected according to the purpose, and it is preferably from 0.4 m / sec to 2.0 m / sec, more preferably from 0.7 m / sec to 1.5 m / sec.
[0215] The volume average particle diameter of the dispersion (oil droplets) in the fine particle dispersion liquid is not particularly limited and can be appropriately selected according to the purpose, and it is preferably from 50 nm to 2,000 nm, more preferably from 50 nm to 500 nm.
[0216] <Desolvation Step> The desolvation step is a step of removing the organic solvent from the fine particle dispersion liquid obtained in the phase inversion emulsification step to obtain base particles.
[0217] The method for removing the organic solvent from the fine particle dispersion liquid is not particularly limited and can be appropriately selected according to the purpose, and examples thereof include a method of gradually raising the temperature of the entire reaction system to evaporate the organic solvent in the fine particle dispersion liquid (oil droplets); a method of spraying the fine particle dispersion liquid into a dry atmosphere to remove the organic solvent in the fine particle dispersion liquid (oil droplets); a method of reducing the pressure of the fine particle dispersion liquid to evaporate and remove the organic solvent. These may be used alone or in combination of two or more kinds.
[0218] The dry atmosphere into which the fine particle dispersion liquid is sprayed is not particularly limited and can be appropriately selected according to the purpose, and examples thereof include gases obtained by heating air, nitrogen, carbon dioxide gas, combustion gas and the like, and various air streams heated to a temperature equal to or higher than the boiling point of the highest boiling point solvent used are generally used.
[0219] The desolvation step can be carried out using an apparatus, for example, a spray dryer, a belt dryer, or a rotary kiln can be used, and sufficient target quality can be obtained in a short-time treatment.
[0220] <c) Aggregation Step> The aforementioned aggregation step involves aggregating the particles of the oil-in-water dispersion to obtain aggregated particles, and then adding an amorphous polyester resin to obtain resin particles. If the method for producing the resin particles includes the solvent removal step, the aggregation step may be a step in which, after obtaining the matrix particles obtained in the solvent removal step, an amorphous polyester resin is added to obtain the resin particles.
[0221] There are no particular limitations on the method for agglomerating the oil droplets or the matrix particles, and a known method can be appropriately selected depending on the purpose. Examples include adding a flocculant or adjusting the pH.
[0222] The flocculant is not particularly limited and can be appropriately selected according to the purpose. Examples thereof include aluminum chloride, zinc sulfate, magnesium sulfate, aluminum sulfate, potassium aluminum sulfate, sodium chloride, sodium bromide, sodium iodide, sodium fluoride, sodium acetate, sodium acetoacetate, lithium chloride, lithium bromide, lithium iodide, lithium fluoride, lithium acetate, lithium acetoacetate, potassium chloride, potassium bromide, potassium iodide, potassium fluoride, potassium acetoacetate, magnesium bromide, magnesium chloride, magnesium iodide, magnesium fluoride, magnesium acetate, magnesium acetoacetate, calcium chloride, calcium bromide, barium bromide, barium chloride, barium iodide, barium fluoride, barium acetate, barium acetoacetate, strontium bromide, strontium chloride, strontium iodide, strontium fluoride, strontium acetate, strontium acetoacetate, zinc bromide, zinc chloride, zinc iodide, zinc fluoride, zinc acetate, zinc acetoacetate, copper bromide, copper chloride, copper iodide, copper fluoride, copper acetate, copper acetoacetate, iron bromide, iron chloride, iron iodide, iron fluoride, iron acetate, and iron acetoacetate. These may be used alone or in combination of two or more. Among these, as the flocculant, a divalent metal salt is preferable, and a trivalent metal salt is more preferable. By using a divalent or higher valent metal salt, a three-dimensional structure can be formed through metal crosslinking with the carboxyl groups contained in the amorphous polyester resin A and the amorphous polyester resin B, which increases the strength of the resin particles and improves the filming resistance.
[0223] When the flocculant is added, it may be added as it is, but it is preferable to prepare an aqueous solution of the flocculant because local high concentration can be avoided. In addition, it is preferable to gradually add the flocculating salt while monitoring the particle size of the resin particles.
[0224] There are no particular restrictions on the temperature of the reaction system in which the agglomeration process is carried out (temperature of the dispersion during agglomeration), and it can be appropriately selected according to the purpose, but it is preferable that it be near the glass transition temperature (Tg) of the amorphous polyester resin B. If the temperature is too low, agglomeration will not proceed well and the efficiency may be poor, and if the temperature is too high, the agglomeration rate will be too fast and the particle size distribution may deteriorate, such as the generation of coarse particles.
[0225] The aggregation process stops after the aggregated particles reach the desired particle size. There are no particular restrictions on the method for stopping the coagulation, and it can be appropriately selected depending on the purpose. For example, methods such as adding a salt or chelating agent with a lower ionic charge than the coagulating salt; adjusting the pH; lowering the temperature of the reaction system (dispersion) during coagulation; or diluting the concentration of the reaction system (dispersion) during coagulation by adding a large amount of aqueous medium can be used. These may be used individually or in combination of two or more.
[0226] There are no particular restrictions on the volume-average particle size of the aggregated particles, and they can be appropriately selected depending on the purpose, but 3.0 μm to 6.0 μm is preferred, and 4.0 μm to 5.0 μm is more preferred.
[0227] In the aggregation step, a mold release agent may be added, and the crystalline resin may be added for low-temperature fixation. As the release agent, you can use the one described in the section on "Release Agent" (for resin particles and toner resin particles) above. When adding the mold release agent or the crystalline resin in the aforementioned aggregation process, a dispersion of the mold release agent in an aqueous medium, or a dispersion of the crystalline polyester resin C, can be prepared and mixed with the fine particle dispersion (oil droplets) before aggregation, thereby obtaining aggregated particles in which the mold release agent or crystalline resin is uniformly dispersed.
[0228] There are no particular restrictions on the particle size of the release agent dispersed in the dispersion, and it can be appropriately selected depending on the purpose, but it is preferably 50 nm to 600 nm, and more preferably 50 nm to 300 nm. In this specification, the particle size of the release agent dispersed in the dispersion is the volume-average particle size.
[0229] The dispersed particle size of the mold release agent can be measured, for example, using a NanoTrac particle size distribution analyzer (UPA-EX150, Nikkiso Co., Ltd., dynamic light scattering method / laser Doppler method) in the same manner as the dispersed particle size of the crystalline resin.
[0230] Furthermore, in order to form a shell layer on the resin particles, a dispersion of the amorphous polyester resin B is added during the aggregation process. By forming a shell layer on the resin particles, the crystalline resin and the release agent that would otherwise worsen the filming properties can be encapsulated, thereby improving filming resistance.
[0231] There are no particular restrictions on the particle size of the amorphous polyester resin B dispersed in the dispersion, and it can be appropriately selected depending on the purpose, but it is preferably 10 nm to 150 nm, and more preferably 10 nm to 70 nm. In this specification, the particle size of the amorphous polyester resin B dispersed in the dispersion is the volume-average particle size.
[0232] The dispersed particle size of the amorphous polyester resin B can be measured, for example, using a NanoTrac particle size distribution analyzer (UPA-EX150, Nikkiso Co., Ltd., dynamic light scattering method / laser Doppler method) in the same manner as the dispersed particle size of the crystalline resin.
[0233] There are no particular limitations on the method for forming the shell layer, and it can be appropriately selected depending on the purpose. For example, one method is to produce aggregated particles using the method described above, and then add the amorphous resin.
[0234] <Fusing process> The aforementioned fusion process is a process of fusing the aggregated particles to reduce irregularities and obtain spherical resin particles.
[0235] There are no particular limitations on the method for fusing the aggregated particles, and it can be appropriately selected depending on the purpose. For example, one method is to heat the dispersion of the aggregated particles while stirring it.
[0236] There are no particular restrictions on the heating temperature, and it can be appropriately selected depending on the purpose, but it is preferably between Tg and Tg+20°C of the amorphous polyester resin B, and more preferably between Tg and Tg+10°C. When the heating temperature is below Tg+20°C of the amorphous polyester resin B, the amorphous polyester resin and the crystalline resin become appropriately compatible, the major axis of the domains during recrystallization of the crystalline resin does not become too large, and it becomes less likely to be exposed on the surface of the resin particles.
[0237] There are no particular restrictions on the average circularity of the resin particles, and they can be appropriately selected depending on the purpose. However, a higher average circularity of the resin particles is preferable, as it allows them to rotate more smoothly in the developing nip when used as toner, thus enabling more resin particles to transfer to the electrostatic latent image carrier. In this respect, a circularity of 0.95 or higher is preferable, and 0.96 or higher is more preferable.
[0238] -Measuring average circularity- In this embodiment, the average particle size and average circularity can be measured, for example, using a flow-type particle image analyzer (FPIA-3000, manufactured by Sysmex Corporation). The specific measurement method involves adding 0.1 mL to 0.5 mL of a surfactant, preferably alkylbenzene sulfonate, as a dispersant to 100 mL to 150 mL of water from which impurities have been removed beforehand, and then adding approximately 0.1 g to 0.5 g of the sample to be measured. The suspension in which the sample is dispersed is subjected to dispersion treatment in an ultrasonic disperser for approximately 1 to 3 minutes, and the dispersion concentration is set to 3,000 particles / μL to 10,000 particles / μL. The average particle size, average roundness, and standard deviation (SD) of roundness are then measured using the aforementioned apparatus. However, the particle size is defined as the equivalent diameter of a circle, the average particle size is determined by the equivalent diameter of a circle (based on the number of particles), and the analysis conditions for the flow-type particle image analyzer are as follows. [Analysis conditions] Particle size limit: 0.5 μm ≤ Equivalent circle diameter (based on number of particles) ≤ 200.0 μm Particle shape limitation: 0.93 < Circularity ≤ 1.00 Furthermore, in this embodiment, the definition of average circularity is as follows: (Average circularity) = (Perimeter of a circle equal to the projected area of the particle) / (Perimeter of the projected image of the particle)
[0239] <Washing Process> The washing step is a step of washing the resin particles obtained in the aggregation step or the fusion step. Since the dispersion of resin particles obtained by the method described above may contain auxiliary materials such as flocculants in addition to the resin particles, it is preferable to wash the dispersion to separate only the resin particles.
[0240] There are no particular restrictions on the method for washing the resin particles, and it can be appropriately selected depending on the purpose. Examples include centrifugal separation, vacuum filtration, or filter pressing. A cake of resin particles can be obtained by any of the washing methods, but if the cake cannot be sufficiently washed in one operation, the obtained cake may be dispersed again in an aqueous solvent to form a slurry, and the process of extracting the resin particles may be repeated using at least one of the washing methods. When washing is performed by the vacuum filtration method or the filter press method, a method may be used in which an aqueous solvent is passed through the cake body to wash away the auxiliary materials that the resin particles have incorporated.
[0241] The aqueous solvent used in the cleaning step is not particularly limited and can be appropriately selected depending on the purpose. Examples include water or a mixed solvent of water and alcohol. Examples of the alcohol include methanol or ethanol. Among these, water is preferred as the aqueous solvent due to its cost and environmental impact from wastewater treatment.
[0242] <Drying process> The drying step is a step of washing the resin particles obtained in the washing step. Since the resin particles washed in the washing step contain a large amount of the aqueous medium, drying them in the drying step removes the aqueous medium, allowing only the resin particles to be obtained.
[0243] There are no particular restrictions on the drying method, and it can be appropriately selected depending on the purpose. Examples include using a spray dryer, vacuum freeze dryer, reduced pressure dryer, stationary shelf dryer, mobile shelf dryer, fluidized bed dryer, rotary dryer, or agitated dryer.
[0244] There are no particular restrictions on the final moisture content of the dried resin particles, and it can be appropriately selected depending on the purpose, but it is preferable that the moisture content be less than 1% by mass.
[0245] The resin particles dried in the aforementioned drying process are soft and aggregated. If this causes problems during use, they may be crushed to break up the aggregates. There are no particular restrictions on the method of crushing, and it can be appropriately selected depending on the purpose. Examples include using a jet mill, Henschel mixer, super mixer, coffee mill, Oster blender, or food processor.
[0246] <Classification process> The classification process is a process of classifying the resin particles obtained in the washing process or the drying process. There are no particular restrictions on the classification method, and it can be appropriately selected depending on the purpose. Examples include methods that remove fine particles in a liquid using a cyclone, decanter, centrifugation, etc., or methods that perform known classification operations after drying.
[0247] <Annealing Process> The annealing step is performed after the drying step when a crystalline resin is added, and is a step that separates the crystalline resin from the amorphous polyester resin.
[0248] There are no particular restrictions on the method of performing the annealing treatment, and it can be appropriately selected depending on the purpose, but examples include storing the crystalline resin at a temperature near its glass transition temperature (Tg) for 10 hours or more.
[0249] In the aforementioned fusion process, if the resin used is heated to a temperature near the glass transition temperature (Tg), the crystalline resin and the amorphous polyester resin may become miscible, making it impossible to achieve both heat resistance and low-temperature fixation. However, the annealing treatment is advantageous because it promotes phase separation between the crystalline resin and the amorphous resin, eliminating the miscible state.
[0250] (toner) The toner of the present invention preferably contains the resin particles for toner of the present invention, and further contains an external additive, and may contain other components as needed.
[0251] <Resin particles for toner> The aforementioned resin particles for toner are as described in the section above (Resin Particles and Resin Particles for Toner), and their details are omitted. In the aforementioned toner, the resin particles for the toner become the toner matrix particles.
[0252] There are no particular restrictions on the content of the toner resin particles in the toner, and it can be appropriately selected depending on the purpose. The toner may also be the toner resin particles themselves.
[0253] <External additives> There are no particular restrictions on the external additives, and they can be appropriately selected depending on the purpose. Examples include inorganic fine particles, oxide fine particles, fatty acid metal salts, or hydrophobized versions thereof. These may be used individually or in combination of two or more.
[0254] There are no particular restrictions on the average particle size of the primary particles of the inorganic fine particles, and it can be appropriately selected depending on the purpose, but it is preferably 100 nm or less, more preferably 1 nm to 100 nm, even more preferably 3 nm to 70 nm, and particularly preferably 5 nm to 70 nm. If the average particle size of the primary particles of the inorganic fine particles is 1 nm or more, it is possible to prevent the inorganic fine particles from becoming embedded in the toner and not being able to effectively perform their function, and if it is 100 nm or less, it is possible to suppress uneven scratching of the photoreceptor surface.
[0255] Furthermore, it is preferable that the inorganic fine particles include at least one type of inorganic fine particles with an average primary particle size of 20 nm or less, and at least one type of inorganic fine particles with an average primary particle size of 30 nm or more.
[0256] There are no particular restrictions on the specific surface area of the inorganic fine particles obtained by the BET method, and it can be appropriately selected according to the purpose, but 20m 2 / g or more 500m 2 It is preferable that the value be less than or equal to / g.
[0257] The inorganic fine particles are not particularly limited and can be appropriately selected depending on the purpose. Examples include silica, alumina, titanium oxide, barium titanate, magnesium titanate, calcium titanate, strontium titanate, iron oxide, copper oxide, zinc oxide, tin oxide, silica sand, clay, mica, wollastonite, diatomaceous earth, chromium oxide, cerium oxide, red iron oxide, antimony trioxide, magnesium oxide, zirconium oxide, barium sulfate, barium carbonate, calcium carbonate, silicon carbide, or silicon nitride. These may be used individually or in combination of two or more. Among these, silica or titanium dioxide are preferred.
[0258] There are no particular limitations on the oxide fine particles, and they can be appropriately selected depending on the purpose. Examples include titania, alumina, tin oxide, or antimony oxide.
[0259] Examples of the fatty acid metal salt include zinc stearate or aluminum stearate.
[0260] Among these, hydrophobized silica, titania, titanium dioxide, or alumina fine particles are preferred as the external additive.
[0261] Examples of the silica nanoparticles mentioned above include R972, R974, RX200, RY200, R202, R805, or R812 (all manufactured by Nippon Aerosil Co., Ltd.).
[0262] Examples of the titania particles include P-25 (manufactured by Nippon Aerosil Co., Ltd.), STT-30, STT-65C-S (all manufactured by Titanium Industry Co., Ltd.), TAF-140 (manufactured by Fuji Titanium Industry Co., Ltd.), MT-150W, MT-500B, MT-600B, or MT-150A (all manufactured by Teika Co., Ltd.).
[0263] Examples of the hydrophobized titanium oxide nanoparticles include T-805 (manufactured by Nippon Aerosil Co., Ltd.), STT-30A, STT-65S-S (all manufactured by Titanium Industry Co., Ltd.), TAF-500T, TAF-1500T (both manufactured by Fuji Titanium Industry Co., Ltd.), MT-100S, MT-100T (both manufactured by Teika Co., Ltd.), or IT-S (manufactured by Ishihara Sangyo Co., Ltd.).
[0264] The hydrophobized oxide nanoparticles, hydrophobized silica nanoparticles, hydrophobized titania nanoparticles, or hydrophobized alumina nanoparticles can be obtained, for example, by treating hydrophilic nanoparticles with a silane coupling agent such as methyltrimethoxysilane, methyltriethoxysilane, or octyltrimethoxysilane. Silicone oil-treated oxide nanoparticles and inorganic nanoparticles obtained by treating silicone oil with heat if necessary are also suitable. Furthermore, the external additive can also be surface-treated with the fluidity improver described above (for resin particles and toner resin particles).
[0265] The silicone oil is not particularly limited and can be appropriately selected depending on the purpose. Examples include dimethyl silicone oil, methylphenyl silicone oil, chlorophenyl silicone oil, methyl hydrogen silicone oil, alkyl-modified silicone oil, fluorine-modified silicone oil, polyether-modified silicone oil, alcohol-modified silicone oil, amino-modified silicone oil, epoxy-modified silicone oil, epoxy-polyether-modified silicone oil, phenol-modified silicone oil, carboxyl-modified silicone oil, mercapto-modified silicone oil, methacrylic-modified silicone oil, or α-methylstyrene-modified silicone oil.
[0266] There are no particular restrictions on the content of the external additive, and it can be appropriately selected depending on the purpose, but it is preferably 0.1 to 5 parts by mass, and more preferably 0.3 to 3 parts by mass, per 100 parts by mass of toner.
[0267] There are no particular restrictions on the method for manufacturing the toner, and any known method can be appropriately selected; however, it is preferable that the toner be manufactured by the method for manufacturing toner of the present invention, which will be described later.
[0268] (Toner manufacturing method) The toner manufacturing method of the present invention includes a mixing step of mixing the toner resin particles of the present invention with an external additive, and further includes other steps as necessary.
[0269] The resin particles are as described in the section (Resin Particles and Resin Particles for Toner), and the external additives are as described in the section (External Additives) of (Toner), and their details are omitted.
[0270] <Mixing process> The mixing step involves mixing the toner resin particles, which serve as the toner matrix particles, with the external additive. Applying a mechanical impact force at this stage is preferable because it can suppress the detachment of the external additive particles from the surface of the toner matrix particles.
[0271] There are no particular limitations on the method of applying the mechanical impact force, and it can be appropriately selected depending on the purpose. Examples include a method of applying impact force to the mixture of the toner resin particles and the external additive using a blade that rotates at high speed; and a method of introducing the mixture of the toner resin particles and the external additive into a high-speed airflow, accelerating it, and causing the particles to collide with each other or with a suitable impact plate.
[0272] There are no particular restrictions on the devices used in the method of applying the aforementioned mechanical impact force, and they can be appropriately selected according to the purpose. Examples include an Ongmill (manufactured by Hosokawa Micron Corporation), a modified I-type mill (manufactured by Nippon Pneumatic Mfg. Co., Ltd.) with reduced grinding air pressure, a hybridization system (manufactured by Nara Machinery Works Co., Ltd.), a cryptron system (manufactured by Kawasaki Heavy Industries, Ltd.), and an automatic mortar and pestle.
[0273] (Developer) The developer of the present invention contains at least the toner of the present invention, and further contains other components that are appropriately selected, such as a carrier, as needed. The toner contained in the developer of the present invention contains the resin particles for toner of the present invention, and therefore the developer makes a significant contribution to carbon neutrality and has excellent low-temperature fixing properties and filming resistance. For this reason, the developer has excellent transferability and electrostatic properties, and can stably form high-quality images.
[0274] The developer may be a one-component developer or a two-component developer, but when used in high-speed printers and the like to accommodate the recent increase in information processing speed, a two-component developer is preferred because it extends the lifespan.
[0275] When the developer is used as a single-component developer, even when the toner is balanced, the particle size of the toner changes little, there is less toner filming on the developing roller and less toner fusion to components such as blades that thin the toner, and good and stable developability and images can be obtained even with long-term agitation in the developing device.
[0276] When the aforementioned developer is used as a two-component developer, even with long-term toner balance, the toner particle size fluctuates little, and good and stable developability and images can be obtained even with long-term agitation in the developing device.
[0277] <Career> There are no particular restrictions on the carrier, and it can be appropriately selected according to the purpose, but one having a core material and a resin layer covering the core material is preferred.
[0278] <<Core material>> There are no particular restrictions on the core material, and it can be appropriately selected according to the purpose. For example, manganese-strontium materials with a magnetization of 50 emu / g to 90 emu / g, or manganese-magnesium materials with a magnetization of 50 emu / g to 90 emu / g are examples. Furthermore, in order to ensure image density, it is preferable to use highly magnetized materials such as iron powder of 100 emu / g or more, or magnetite with a magnetization of 75 emu / g to 120 emu / g. In addition, it is preferable to use low magnetized materials such as copper-zinc materials with a magnetization of 30 emu / g to 80 emu / g, as this can mitigate the impact of the developer in a condensed state on the photoreceptor and is advantageous for improving image quality. These can be used individually or in combination of two or more.
[0279] There are no particular restrictions on the volume-average particle size of the core material, and it can be appropriately selected according to the purpose, but it is preferably 10 μm to 150 μm, and more preferably 40 μm to 100 μm. When the volume-average particle size of the core material is 10 μm or more, it is possible to prevent a large amount of fine powder from accumulating in the carrier, and to suppress the decrease in magnetization per particle and the resulting scattering of carriers. Furthermore, when the volume-average particle size of the core material is 150 μm or less, it is possible to prevent a decrease in specific surface area and toner scattering, and in full-color printing with many solid areas, it is possible to suppress poor reproduction of solid areas in particular.
[0280] When the toner is used in a two-component developer, it may be used in combination with the carrier. There are no particular restrictions on the amount of the carrier in the two-component developer, and it can be appropriately selected depending on the purpose, but it is preferably 90 parts by mass or more and 98 parts by mass or less, and more preferably 93 parts by mass or more and 97 parts by mass or less, per 100 parts by mass of the two-component developer.
[0281] The developer can be suitably used for image formation by various known electrophotographic methods, including magnetic one-component development methods, non-magnetic one-component development methods, or two-component development methods.
[0282] (Image forming apparatus and image forming method) The image forming apparatus of the present invention comprises an electrostatic latent image carrier, an electrostatic latent image forming means for forming an electrostatic latent image on the electrostatic latent image carrier, and a developing means comprising a toner for developing the electrostatic latent image formed on the electrostatic latent image carrier to form a visible image, and further comprises other means as necessary. The toner in the developing means is the toner of the present invention.
[0283] The image forming method of the present invention includes an electrostatic latent image forming step of forming an electrostatic latent image on an electrostatic latent image carrier, and a developing step of developing the electrostatic latent image formed on the electrostatic latent image carrier using toner to form a visible image, and further includes other steps as necessary. The toner in the developing step is the toner of the present invention.
[0284] The image forming method can be suitably carried out by the image forming apparatus, the electrostatic latent image forming step can be suitably carried out by the electrostatic latent image forming means, the developing step can be suitably carried out by the developing means, and the other steps can be suitably carried out by the other means.
[0285] <Electrostatic latent image carrier> There are no particular restrictions on the material, structure, or size of the electrostatic latent image carrier (hereinafter sometimes referred to as the "photoreceptor"), and they can be appropriately selected from known materials. Examples of materials for the electrostatic latent image carrier include inorganic photoreceptors and organic photoreceptors. Examples of the inorganic photoreceptor include amorphous silicon or selenium. Examples of the organic photoreceptor include polysilane or phthalopolymethine. Among these, amorphous silicon is preferred as the electrostatic latent image carrier in terms of its long lifespan.
[0286] As the amorphous silicon photoreceptor, for example, a photoreceptor having a photoconductive layer made of a-Si can be used by heating a support to 50°C to 400°C and depositing it on the support using a film deposition method such as vacuum deposition, sputtering, ion plating, thermal CVD (chemical vapor deposition), photo-CVD, or plasma CVD. Among these film deposition methods, plasma CVD, that is, a method in which a source gas is decomposed by DC, high-frequency, or microwave glow discharge to form an a-Si deposited film on the support, is preferred.
[0287] There are no particular restrictions on the shape of the electrostatic latent image carrier, and it can be appropriately selected depending on the purpose, but a cylindrical shape is preferred. There are no particular restrictions on the outer diameter of the cylindrical electrostatic latent image carrier, and it can be appropriately selected depending on the purpose, but it is preferably 3 mm to 100 mm, more preferably 5 mm to 50 mm, and particularly preferably 10 mm to 30 mm.
[0288] <Electrostatic latent image forming means and electrostatic latent image forming process> The electrostatic latent image forming means is a means for forming an electrostatic latent image on the electrostatic latent image carrier. The electrostatic latent image formation step is a step of forming an electrostatic latent image on the electrostatic latent image carrier. The electrostatic latent image formation step is preferably carried out by the electrostatic latent image formation means.
[0289] The electrostatic latent image forming means is not particularly limited and can be appropriately selected depending on the purpose. For example, it may include a means having at least a charging member for charging the surface of the electrostatic latent image carrier and an exposure member for exposing the surface of the electrostatic latent image carrier to an image.
[0290] The electrostatic latent image formation step is not particularly limited and can be appropriately selected depending on the purpose. For example, it can be performed by charging the surface of the electrostatic latent image carrier and then exposing it to light in an image-like manner.
[0291] <<Charging material and charging>> There are no particular restrictions on the charging member, and it can be appropriately selected from known ones depending on the purpose. Examples include contact chargers, Corotrons, or non-contact chargers that utilize corona discharge such as Scorotrons. The contact charger preferably includes conductive or semiconducting rollers, brushes, films, or rubber blades.
[0292] The charging can be performed, for example, by applying a voltage to the surface of the electrostatic latent image carrier using the charging member.
[0293] The shape of the charging member can be any form other than a roller, such as a magnetic brush or a fur brush, and can be selected according to the specifications and configuration of the image forming apparatus. The charging member is not limited to the contact-type charging member, but it is preferable to use a contact-type charging member because it reduces the amount of ozone generated from the charging member, thus providing an image forming apparatus with reduced ozone emissions.
[0294] <<Exposure component and exposure>> The exposure member is not particularly limited as long as it can expose the surface of the electrostatic latent image carrier, which has been charged by the charging member, in the manner of the image to be formed. It can be appropriately selected according to the purpose, and examples include various exposure members such as copying optical systems, rod lens array systems, laser optical systems, or liquid crystal shutter optical systems.
[0295] There are no particular restrictions on the light source used in the exposure member, and it can be appropriately selected according to the purpose. Examples include fluorescent lamps, tungsten lamps, halogen lamps, mercury lamps, sodium lamps, light-emitting diodes (LEDs), semiconductor lasers (LDs), or light-emitting materials in general such as electroluminescent devices (ELs).
[0296] Furthermore, various filters such as sharp-cut filters, band-pass filters, near-infrared cut filters, dichroic filters, interference filters, or color temperature conversion filters can be used to irradiate only light in the desired wavelength range.
[0297] The exposure can be performed, for example, by exposing the surface of the electrostatic latent image carrier in an image-like manner using the exposure member. In addition, in the present invention, a back-facing method may be employed in which the electrostatic latent image carrier is exposed in an image-like manner from the back side.
[0298] <Developing means and developing process> The developing means comprises a toner that develops the electrostatic latent image formed on the electrostatic latent image carrier to form a visible image. The development step is a step of developing the electrostatic latent image formed on the electrostatic latent image carrier using toner to form a visible image. The development step is preferably carried out by the developing means.
[0299] The developing means is not particularly limited and can be appropriately selected according to the purpose, and may be a dry developing method or a wet developing method. Furthermore, the developing means may be a single-color developing means or a multi-color developing means. Among these, a developing apparatus is preferred, which has an agitator that frictionally agitates and charges the toner, a magnetic field generating means fixed inside, and a developer carrier on its surface that is rotatable and carries a developer containing the toner.
[0300] Within the developing means, for example, the toner and carrier are mixed and stirred, and the friction during this process causes the toner to become charged, which is then held in a brush-like state on the surface of a rotating magnetic roller, forming a magnetic brush. The magnetic roller is positioned near the electrostatic latent image carrier. Therefore, a portion of the toner that constitutes the magnetic brush formed on the surface of the magnetic roller moves to the surface of the electrostatic latent image carrier by electrical attraction. As a result, the electrostatic latent image is developed by the toner, and a visible image is formed on the surface of the electrostatic latent image carrier by the toner.
[0301] Here, there are no particular restrictions on the carrier, and it can be appropriately selected according to the purpose. For example, those listed in the (developer) section above can be used.
[0302] <Other means and other processes> The aforementioned other means are not particularly limited and can be appropriately selected depending on the purpose. Examples include transfer means, fixing means, cleaning means, static elimination means, recycling means, or control means. The aforementioned other processes are not particularly limited and can be appropriately selected depending on the purpose. Examples include a transfer process, a fixing process, a cleaning process, a static elimination process, a recycling process, or a control process.
[0303] <<Transfer means and transfer process>> The transfer means is a means for transferring the visible image formed by the developing means onto a recording medium. The transfer step is a step of transferring the visible image formed in the development step onto a recording medium. The transfer step is preferably carried out by the transfer means.
[0304] There are no particular limitations on the transfer means, and they can be appropriately selected according to the purpose, but an embodiment having a first transfer means for transferring the visible image onto an intermediate transfer medium to form a composite transfer image, and a second transfer means for transferring the composite transfer image onto a recording medium is preferred.
[0305] The transfer step is not particularly limited and can be appropriately selected depending on the purpose, but a preferred method is to use an intermediate transfer body, first transfer the visible image onto the intermediate transfer body, and then second transfer the visible image onto the recording medium. Specifically, the transfer step can be performed, for example, by charging the photoreceptor using a transfer charger, and can be performed by the transfer means.
[0306] In this configuration, if the image to be secondarily transferred onto the recording medium is a color image consisting of multiple toners, the transfer means can sequentially superimpose each toner onto the intermediate transfer body to form an image on the intermediate transfer body, and the intermediate transfer means can then secondarily transfer the image on the intermediate transfer body onto the recording medium in one go. There are no particular restrictions on the intermediate transfer material, and it can be appropriately selected from known transfer materials depending on the purpose. For example, a transfer belt is a suitable example.
[0307] The transfer means (the primary transfer means, the secondary transfer means) preferably includes at least a transfer device that exfoliates and charges the visible image formed on the photoreceptor toward the recording medium. There are no particular limitations on the transfer device, and it can be appropriately selected according to the purpose. Examples include corona discharge transfer devices, transfer belts, transfer rollers, pressure transfer rollers, or adhesive transfer devices.
[0308] While plain paper is a typical recording medium, there are no particular restrictions as long as it can transfer the unfixed image after development. It can be appropriately selected according to the purpose, and PET bases for OHPs can also be used.
[0309] <<Fixing means and fixing process>> The fixing means is a means for fixing the transferred image transferred to the recording medium. The fixing step is a step of fixing the transferred image that has been transferred to the recording medium. The fixing process is preferably carried out by the fixing means.
[0310] The fixing means is not particularly limited and can be appropriately selected depending on the purpose, but a known heating and pressing member is preferred. There are no particular restrictions on the heating and pressing member, and it can be appropriately selected according to the purpose. Examples include a combination of a heating roller and a pressing roller, or a combination of a heating roller, a pressing roller and an endless belt. In addition, in the present invention, depending on the purpose, a known optical fuser may be used together with or instead of the fixing means, for example.
[0311] There are no particular restrictions on the fixing process, and it can be appropriately selected according to the purpose. For example, it may be performed each time the toner of each color is transferred to the recording medium, or it may be performed simultaneously on all the toners at once while they are stacked.
[0312] There are no particular restrictions on the heating temperature of the heating and pressurizing member, and it can be appropriately selected depending on the purpose, but 80°C to 200°C is preferred.
[0313] There are no particular restrictions on the surface pressure in the fixing process, and it can be appropriately selected according to the purpose, but 10 N / cm is recommended. 2 More than 80N / cm 2 The following is preferable:
[0314] <<Cleaning Methods and Cleaning Processes>> The cleaning means is a means for removing the toner remaining on the photoreceptor. The cleaning step is a step of removing the toner remaining on the photoreceptor. The cleaning process is preferably carried out by the cleaning means.
[0315] The cleaning means is not particularly limited and can be appropriately selected depending on the purpose. Examples include a magnetic brush cleaner, an electrostatic brush cleaner, a magnetic roller cleaner, a blade cleaner, a brush cleaner, or a web cleaner.
[0316] <<Static elimination means and static elimination process>> The static elimination means is a means of eliminating static electricity by applying a static elimination bias to the photoreceptor. The static elimination step is a step of eliminating static electricity by applying a static elimination bias to the photoreceptor. The static elimination process is preferably carried out by the static elimination means.
[0317] There are no particular restrictions on the static elimination means, and they can be appropriately selected according to the purpose. For example, static elimination lamps can be used.
[0318] <<Recycling methods and recycling processes>> The recycling means is a means for transporting the toner removed by the cleaning means to the developing means for recycling. The recycling process involves transporting the toner removed in the cleaning process to the developing process for recycling. The recycling process is preferably carried out by the recycling means.
[0319] There are no particular restrictions on the recycling means, and they can be appropriately selected depending on the purpose. Examples include known transport means.
[0320] <<Control means and control process>> The control means is a means for controlling the movement of each of the means. The control step is a step that controls the movement of each of the steps. The control step is preferably performed by the control means.
[0321] The control means are not particularly limited and can be appropriately selected depending on the purpose. Examples include a sequencer or a computer.
[0322] Next, an embodiment of the image forming apparatus and the image forming method of the present invention will be described with reference to Figures 2 to 5. The color image forming apparatus 100A shown in Figure 2 comprises a photoreceptor drum 10 (hereinafter sometimes referred to as "photoreceptor 10") as the electrostatic latent image carrier, a charging roller 20 as the charging means, an exposure apparatus 30 as the exposure means, a developer 40 as the developing means, an intermediate transfer body 50, a cleaning apparatus 60 as the cleaning means having a cleaning blade, and a static elimination lamp 70 as the static elimination means.
[0323] The intermediate transfer body 50 is an endless belt and is designed to be movable in the direction of the arrow by three rollers 51 positioned inside it and tensioning it. Part of the three rollers 51 also function as transfer bias rollers capable of applying a predetermined transfer bias (primary transfer bias) to the intermediate transfer body 50. A cleaning device 90 having a cleaning blade is positioned near the intermediate transfer body 50. Also positioned near the intermediate transfer body 50, facing the intermediate transfer body 50, is a transfer roller 80, which is a transfer means capable of applying a transfer bias for transferring a developed image (toner image) to a transfer paper 95, which is a recording medium (secondary transfer). Around the intermediate transfer body 50, a corona charger 58 for imparting an electric charge to the toner image on the intermediate transfer body 50 is positioned between the contact area between the photoreceptor 10 and the intermediate transfer body 50 and the contact area between the intermediate transfer body 50 and the transfer paper 95 in the rotational direction of the intermediate transfer body 50.
[0324] The developing unit 40 consists of a developing belt 41 as a developer carrier, and a black developing unit 45K, a yellow developing unit 45Y, a magenta developing unit 45M, and a cyan developing unit 45C, all of which are arranged around the developing belt 41. The black developing unit 45K includes a developer storage section 42K, a developer supply roller 43K, and a developing roller 44K. The yellow developing unit 45Y includes a developer storage section 42Y, a developer supply roller 43Y, and a developing roller 44Y. The magenta developing unit 45M includes a developer storage section 42M, a developer supply roller 43M, and a developing roller 44M. The cyan developing unit 45C includes a developer storage section 42C, a developer supply roller 43C, and a developing roller 44C. The developing belt 41 is an endless belt, rotatably stretched over multiple belt rollers, with a portion of it in contact with the electrostatic latent image carrier 10.
[0325] In the color image forming apparatus 100A shown in Figure 2, for example, a charging roller 20 uniformly charges the photoreceptor drum 10. An exposure device 30 exposes the photoreceptor drum 10 in an image-like manner, forming an electrostatic latent image. The electrostatic latent image formed on the photoreceptor drum 10 is developed by supplying toner from the developer 40 to form a toner image. This toner image is transferred (primary transfer) onto an intermediate transfer body 50 by a voltage applied from a roller 51, and then transferred (secondary transfer) onto a transfer paper 95. As a result, a transferred image is formed on the transfer paper 95. Residual toner on the photoreceptor 10 is removed by a cleaning device 60, and the charge on the photoreceptor 10 is temporarily removed by an anti-static lamp 70.
[0326] Figure 3 shows another example of the image forming apparatus of the present invention. The image forming apparatus 100B has the same configuration as the image forming apparatus 100A shown in Figure 3, except that it does not have a developing belt 41, and the black developing unit 45K, yellow developing unit 45Y, magenta developing unit 45M, and cyan developing unit 45C are arranged directly opposite each other around the photoreceptor drum 10.
[0327] Figure 4 shows another example of the image forming apparatus of the present invention. The image forming apparatus 100C shown in Figure 4 comprises a copy device body 150, a paper feed table 200, a scanner 300, and an automatic document feeder (ADF) 400. The copying device body 150 has an endless belt-shaped intermediate transfer body 50 provided in the center. The intermediate transfer body 50 is stretched over support rollers 14, 15, and 16 and is rotatable clockwise in Figure 4. Near the support roller 15, an intermediate transfer body cleaning device 17 is positioned to remove residual toner from the intermediate transfer body 50. A tandem-type developer 120, in which four image forming means 18 for yellow, cyan, magenta, and black are arranged opposite each other along the transport direction of the intermediate transfer body 50 stretched over the support rollers 14 and 15, is positioned. Near the tandem-type developer 120, an exposure device 21, which is the exposure member, is positioned. On the side of the intermediate transfer body 50 opposite to the side where the tandem-type developer 120 is positioned, a secondary transfer device 22 is positioned. In the secondary transfer device 22, an endless belt, the secondary transfer belt 24, is stretched over a pair of rollers 23, and the transfer paper and the intermediate transfer body 50 being transported on the secondary transfer belt 24 can come into contact with each other. A fixing device 25, which is the fixing means, is located near the secondary transfer device 22. The fixing device 25 comprises a fixing belt 26, which is an endless belt, and a pressure roller 27 that is positioned under pressure from the fixing belt 26. In the tandem image forming apparatus, a sheet reversing device 28 is located near the secondary transfer device 22 and the fixing device 25 to reverse the transfer paper in order to form an image on both sides of the transfer paper.
[0328] Next, the formation of a full-color image (color copy) using the tandem-type developing unit 120 will be described. Specifically, first, the original document is placed on the document glass 130 of the automatic document feeder (ADF) 400, or the automatic document feeder 400 is opened and the original document is placed on the contact glass 32 of the scanner 300, and then the automatic document feeder 400 is closed.
[0329] When the start switch is pressed, if a document is placed in the automatic document transporter 400, the document is transported and moved onto the contact glass 32 before the scanner 300 starts to operate. If a document is placed on the contact glass 32, the scanner 300 starts to operate immediately. The first travel body 33 and the second travel body 34 then move. At this time, the first travel body 33 illuminates the document with light from the light source, and the mirror on the second travel body 34 reflects the reflected light from the document surface. This light is then received by the reading sensor 36 through the imaging lens 35, and the color document (color image) is read and converted into black, yellow, magenta, and cyan image information.
[0330] The image information for black, yellow, magenta, and cyan is then transmitted to each image forming means 18 (image forming means for black, image forming means for yellow, image forming means for magenta, and image forming means for cyan) in the tandem-type developer 120. Then, the toner images for black, yellow, magenta, and cyan are formed in each image forming means.
[0331] Specifically, each image forming means 18 in the tandem-type developer 120 (image forming means for black, image forming means for yellow, image forming means for magenta, and image forming means for cyan) consists of, as shown in Figure 5, an electrostatic latent image carrier 10 (electrostatic latent image carrier 10K for black, electrostatic latent image carrier 10Y for yellow, electrostatic latent image carrier 10M for magenta, and electrostatic latent image carrier 10C for cyan), a charging device 160 which is the charging means for uniformly charging the electrostatic latent image carrier 10, and based on each color image information The system includes an exposure apparatus that exposes the electrostatic latent image carrier to each color image (L in Figure 5) and forms an electrostatic latent image on the electrostatic latent image carrier corresponding to each color image; a developing apparatus 61 which is the developing means that develops the electrostatic latent image using each color toner (black toner, yellow toner, magenta toner, and cyan toner) to form a toner image using each color toner; a transfer charger 62 for transferring the toner image onto an intermediate transfer body 50; a cleaning apparatus 63; and a static eliminator 64.
[0332] Each image forming means 18 is capable of forming a monochrome image (black image, yellow image, magenta image, and cyan image) based on the image information of its respective color. The black image, yellow image, magenta image, and cyan image thus formed are sequentially transferred (primary transfer) onto an intermediate transfer body 50 that is rotated by support rollers 14, 15, and 16, respectively, with the black image formed on the black electrostatic latent image carrier 10K, the yellow image formed on the yellow electrostatic latent image carrier 10Y, the magenta image formed on the magenta electrostatic latent image carrier 10M, and the cyan image formed on the cyan electrostatic latent image carrier 10C. The black image, yellow image, magenta image, and cyan image are then superimposed on the intermediate transfer body 50 to form a composite color image (color transfer image).
[0333] Meanwhile, in the paper feed table 200, one of the paper feed rollers 142 is selectively rotated to feed a sheet (recording paper) from one of the multi-stage paper feed cassettes 144 in the paper bank 143. The sheets are separated one by one by the separation roller 145 and sent to the paper feed path 146, transported by the transport roller 147 and guided to the paper feed path 148 in the copier body 150, where they are stopped by the registration roller 49. Alternatively, the paper feed roller 142 is rotated to feed a sheet (recording paper) from the manual feed tray 54, separate it one by one by the separation roller 52 and put it into the manual feed path 53, where it is stopped by the registration roller 49. The registration roller 49 is generally used in a grounded state, but it may also be used with a bias applied to remove paper dust from the sheets.
[0334] Then, the register roller 49 is rotated in time with the composite color image (color transfer image) synthesized on the intermediate transfer body 50, and a sheet (recording paper) is fed between the intermediate transfer body 50 and the secondary transfer device 22, and the secondary transfer device 22 transfers the composite color image (color transfer image) onto the sheet (recording paper) (secondary transfer). In this way, a color image is transferred and formed on the sheet (recording paper). After image transfer, any residual toner on the intermediate transfer body 50 is cleaned by the intermediate transfer body cleaning device 17.
[0335] The sheet (recording paper) on which the color image has been transferred and formed is transported by the secondary transfer device 22 and sent to the fixing device 25, where the composite color image (color transfer image) is fixed onto the sheet (recording paper) by heat and pressure. After that, the sheet (recording paper) is switched by the switching claw 55 and discharged by the discharge roller 56 and stacked on the paper output tray 57. Alternatively, the sheet is switched by the switching claw 55 and inverted by the sheet inversion device 28 and guided back to the transfer position, where an image is recorded on the back side as well, before being discharged by the discharge roller 56 and stacked on the paper output tray 57.
[0336] (Toner storage unit) The toner storage unit of the present invention is a unit having the function of storing toner, in which toner is stored. The toner contained in the toner storage unit is the toner of the present invention. Therefore, the toner storage unit of the present invention has a low environmental impact. Furthermore, by mounting the toner storage unit in the image forming apparatus of the present invention and performing image formation, image formation is performed using the toner of the present invention, thus achieving both filming resistance and low-temperature fixing performance.
[0337] The configuration of the toner storage unit is not particularly limited as long as it can accommodate the toner, and can be appropriately selected according to the purpose. Examples include a toner storage container, a developer, or a process cartridge.
[0338] <Toner container> The toner container mentioned above refers to a container that contains the toner. The toner storage container is not particularly limited and can be appropriately selected from known types, such as one having a container body and a cap.
[0339] The size of the container body is not particularly limited and can be changed as appropriate.
[0340] The shape of the container body is not particularly limited and can be changed as appropriate, but it is preferably cylindrical.
[0341] The structure of the container body is not particularly limited and can be modified as appropriate, but a structure is preferred in which spiral-shaped irregularities are formed on the inner circumferential surface, and the toner contents can be moved to the discharge port side by rotating the container, and in which part or all of the spiral-shaped irregularities have a bellows function.
[0342] The material of the container body is not particularly limited and can be changed as appropriate, but it is preferable that it has good dimensional accuracy. Examples include resin materials such as polyester resin, polyethylene resin, polypropylene resin, polystyrene resin, polyvinyl chloride resin, polyacrylic acid, polycarbonate resin, ABS resin, or polyacetal resin. These may be used individually or in combination of two or more.
[0343] The toner storage container is easy to store and transport, and has excellent handling properties, so it can be detachably attached to a process cartridge or image forming apparatus and used for replenishing the toner.
[0344] <developer> The term "developer" refers to a device that houses the toner and has a developing mechanism. The developing means is not particularly limited and can be appropriately selected according to the purpose. For example, it may include at least a toner storage container and a toner carrier that carries and transports the toner stored in the toner storage container. Furthermore, the developing means may include regulating members or the like to control the thickness of the toner it carries.
[0345] <Processing Cartridge> The process cartridge refers to a device that integrates at least an electrostatic latent image carrier and a developing means, contains the toner, and is detachable from the image forming apparatus. The process cartridge may further have at least one selected from a charging means, an exposure means, a cleaning means, and a static elimination means, as needed.
[0346] An example of the process cartridge is one which is molded to be detachable from various image forming apparatuses and has at least an electrostatic latent image carrier that carries an electrostatic latent image, and a developing means that develops the electrostatic latent image carried on the electrostatic latent image carrier with the toner to form a toner image, and may have other means as needed.
[0347] Next, an embodiment of the process cartridge is shown in Figure 6. As shown in Figure 6, the process cartridge 110 of this embodiment incorporates an electrostatic latent image carrier 10 and includes a charger 58 as a charging means, a developer 40 as a developing means, and a cleaning device 90 as a cleaning means, and further includes other means as necessary. In Figure 6, the reference numeral L indicates exposure from an exposure means (not shown), and the reference numeral 95 indicates recording paper. The electrostatic latent image carrier 10 can be the same as the electrostatic latent image carrier used in an image forming apparatus. Any charging member can be used for the charger 58. In the image formation process using the process cartridge shown in Figure 6, the electrostatic latent image carrier 10 rotates in the direction of the arrow, and is charged by the charger 58 and exposed by the exposure means L, thereby forming an electrostatic latent image on its surface corresponding to the exposed image. This electrostatic latent image is developed by toner development in the developer unit 40, and the developed toner is transferred to recording paper 95 by the transfer roller 80 and printed out. Next, the surface of the electrostatic latent image carrier 10 after image transfer is cleaned by the cleaning device 90 and further discharged by a static discharge means (not shown), and the above operation is repeated again. [Examples]
[0348] The present invention will be specifically described below with reference to manufacturing examples, preparation examples, examples, and comparative examples, but the present invention is not limited in any way to these manufacturing examples, preparation examples, and examples. In the manufacturing examples, preparation examples, examples, and comparative examples, unless otherwise specified, "%" refers to "mass%" and "parts" refers to "parts by mass". In addition, the blending amounts in the examples and comparative examples indicate the blending amount of solids in each raw material.
[0349] The measured values in the following manufacturing examples, preparation examples, examples, and comparative examples were measured by the method described below.
[0350] <<Measuring Amine Titer>> In the following manufacturing examples, the amine value of the ketimine compound was measured according to the method described in JIS K7237.
[0351] <<Measurement of glass transition temperature (Tg) and melting point (Tm)>> The glass transition temperatures (Tg) of amorphous polyester resin A and amorphous polyester resin B, and the melting point (Tm) of crystalline polyester resin C, obtained in the following manufacturing examples, were measured using a DSC system (differential scanning calorimeter) ("Q-200", manufactured by TA Instruments). First, approximately 5.0 mg of the target sample was placed in an aluminum sample container, which was then placed on a holder unit and set in an electric furnace. Next, under a nitrogen atmosphere, it was heated from -80°C to 150°C at a heating rate of 10°C / min (first heating pass). After that, it was cooled from 150°C to -80°C at a cooling rate of 10°C / min, and then heated again to 150°C at a heating rate of 10°C / min (second heating pass). In both the first and second heating passes, a differential scanning calorimeter ("Q-200", manufactured by TA Instruments Inc.) was used to measure the DSC curve. From the obtained DSC curves, the DSC curve for the second heating cycle was selected using the analysis program in the Q-200 system, and the glass transition temperature of the target sample during the second heating cycle was determined. Furthermore, using the analysis program in the Q-200 system, the DSC curve for the second heating cycle was selected from the obtained DSC curves, and the endothermic peak top temperature of the target sample during the second heating cycle was determined as the melting point.
[0352] <<Measuring Molecular Weight>> The molecular weights of amorphous polyester resin A, amorphous polyester resin B, and crystalline polyester resin C obtained in the following manufacturing examples were measured using a gel permeation chromatography (GPC) analyzer under the following analytical conditions. This was done by dissolving amorphous polyester resin A, amorphous polyester resin B, or crystalline polyester resin C in tetrahydrofuran (THF) (containing stabilizer, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) or chloroform at a concentration of 0.15% by mass, filtering the solution through a 0.2 μm filter, and using the filtrate as the sample. [Analysis conditions] • Gel permeation chromatography (GPC) measuring device: GPC-8220GPC (manufactured by Tosoh Corporation) Column: TSKgel® SuperHZM-H 15cm 3-row (manufactured by Tosoh Corporation) ·Temperature: 40℃ • Detector: RI (refractive index) detector • Solvent: Tetrahydrofuran (THF) or chloroform Flow rate: 0.35 mL / min • Sample: Inject 100 μL of 0.15 mass% of the sample. For molecular weight measurement of the samples, the molecular weight distribution of the samples was calculated from the relationship between the logarithm of a calibration curve prepared using several monodisperse polystyrene standard samples and the count. The standard polystyrene samples used for creating the calibration curve were Showdex® STANDARD (manufactured by Showa Denko K.K.) Std. No. S-6550, S-1700, S-740, S-321, S-129, S-10, S-2.9, and S-0.6.
[0353] <<Measurement of Acid Value>> In the following examples and comparative examples, the acid values of amorphous polyester resin B and crystalline polyester resin C were measured under the following conditions in accordance with the measurement method described in JIS K0070-1992. 0.5 g of each resin (0.3 g for the ethyl acetate-soluble portion) was added to 120 mL of toluene and dissolved by stirring at room temperature (23°C) for approximately 10 hours. Furthermore, 30 mL of ethanol was added to prepare the sample solution. The acid value of the sample solution was measured at 23°C using a potentiometric automatic titrator (DL-53 Titrator, Mettler-Toledo) and an electrode DG113-SC (Mettler-Toledo), and analyzed using the analysis software LabX Light Version 1.00.000. A mixed solvent of 120 mL of toluene and 30 mL of ethanol was used in the apparatus. The measurement can be carried out using the measurement method described above, but the acid value was specifically calculated as follows: The solution was titrated with a pre-standardized 0.1N potassium hydroxide / alcohol solution, and the acid value was determined from the titration volume using the following formula. Acid value [mgKOH / g] = Titration volume [mL] × N × 56.1 [mg / mL] / Sample mass [g] (However, in the above formula, "N" represents the factor of a 0.1N potassium hydroxide / alcohol solution.)
[0354] <<Measurement of hydroxyl value>> In the following examples and comparative examples, the hydroxyl values of amorphous polyester resin B and crystalline polyester resin C were measured under the following conditions in accordance with the measurement method described in JIS K0070-1966. 0.5 g of each resin was accurately weighed into a 100 mL volumetric flask, and 5 mL of acetylation reagent was precisely added to it. Then, the flask was heated in a bath at 100°C ± 5°C. After 1 to 2 hours, the volumetric flask was removed from the bath, allowed to cool, and water was added and shaken to decompose the acetic anhydride. Next, to complete the decomposition, the flask was heated again in the bath for at least 10 minutes, allowed to cool, and the flask walls were thoroughly washed with an organic solvent to obtain the sample solution. Using a potentiometric automatic titrator (DL-53 Titrator, Mettler-Toledo) and electrode DG113-SC (Mettler-Toledo), the sample solution was potentiometrically titrated with an N / 2 potassium hydroxide ethyl alcohol solution at 23°C to measure the hydroxyl value, which was then analyzed using the analysis software LabX Light Version 1.00.000. A mixed solvent of 120 mL of toluene and 30 mL of ethanol was used in the apparatus.
[0355] <<Measurement of volume-average particle size>> The volume-average particle size of the particles contained in the amorphous polyester resin B dispersion, crystalline polyester resin C dispersion, wax dispersion, and solvent-removing slurry 1 obtained in the following preparation examples was measured using a NanoTrac particle size distribution analyzer (UPA-EX150, Nikkiso Co., Ltd., dynamic light scattering method / laser Doppler method). First, background measurements were performed using only the dispersion solvent of each target sample dispersion. Next, the dispersions containing each target sample were adjusted to the measurement concentration range and measured.
[0356] <<Measurement of average circularity>> The average circularity of the particles in the fusion process of the following examples and comparative examples was measured using a flow-type particle image analyzer (FPIA-3000, manufactured by Sysmex Corporation). The average circularity is defined by the following formula. (Average circularity) = (Perimeter of a circle equal to the projected area of the particle) / (Perimeter of the projected image of the particle)
[0357] The specific measurement method involved adding 0.2 mL of a surfactant (alkylbenzene sulfonate) as a dispersant to 100 mL of water from which impurities had been removed beforehand, and then adding 0.1 g of the target sample. Next, the suspension containing the target sample was subjected to dispersion treatment for 2 minutes using an ultrasonic disperser, and the dispersion concentration was adjusted from 3,000 particles / μL to 10,000 particles / μL. The average particle size, average circularity, and standard deviation (SD) of circularity were then measured using a flow-type particle image analyzer (FPIA-3000, manufactured by Sysmex Corporation). However, the particle size was defined as the equivalent diameter of a circle, and the average particle size was determined by the equivalent diameter of a circle (based on the number of particles). The analysis conditions for the flow-type particle image analyzer were as follows. [Analysis conditions] • Particle size limit: 0.5 μm ≤ Equivalent circle diameter (based on number of particles) ≤ 200.0 μm • Particle shape limitation: 0.93 < Circularity ≤ 1.00
[0358] <<Measurement of volume-average particle size (D4) and number-average particle size (Dn) of toner>> The volume-average particle size (D4), number-average particle size (Dn), and their ratio (D4 / Dn) of the toners obtained in the following examples and comparative examples were measured using a Coulter Multisizer II (manufactured by Coulter, Inc.). First, a mixture was obtained by adding 0.1 mL of a surfactant (polyoxyethylene alkyl ether) as a dispersant to 100 mL of an electrolytic aqueous solution (ISOTON-II, manufactured by Coulter). 2 mg of the sample to be measured was then added to this mixture. The electrolytic aqueous solution containing the sample was dispersed using an ultrasonic disperser for 2 minutes. Using the aforementioned measuring device (Coulter Multisizer II) with a 100 μm aperture, the volume and number of each toner particle were measured, and the volume and number distributions were calculated. From the obtained distributions, the volume-average particle size (D4) and number-average particle size (Dn) of each toner particle were determined. Furthermore, from these values, the ratio of volume-average particle size (D4) to number-average particle size (Dn) (D4 / Dn) and the components smaller than 2 μm (number %) were determined.
[0359] Thirteen channels were used, with the following channel sizes: 2.00 μm to less than 2.52 μm, 2.52 μm to less than 3.17 μm; 3.17 μm to less than 4.00 μm, 4.00 μm to less than 5.04 μm, 5.04 μm to less than 6.35 μm, 6.35 μm to less than 8.00 μm, 8.00 μm to less than 10.08 μm, 10.08 μm to less than 12.70 μm, 12.70 μm to less than 16.00 μm, 16.00 μm to less than 20.20 μm, 20.20 μm to less than 25.40 μm, 25.40 μm to less than 32.00 μm, and 32.00 μm to less than 40.30 μm. The target particles were those with a particle size of 2.00 μm to less than 40.30 μm.
[0360] (Manufacturing example 1: Synthesis of ketimine) In a reaction vessel equipped with a stirring rod and thermometer, 170 parts of isophorone diamine and 75 parts of methyl ethyl ketone were charged, and the reaction was carried out at 50°C for 5 hours to obtain [Ketimine Compound 1]. The amine value of [Ketimine Compound 1] was 418 mgKOH / g.
[0361] (Manufacturing Example A-1: Synthesis of Amorphous Polyester Resin A-1) <Synthesis of Prepolymer A-1> In a reaction vessel equipped with a condenser, stirrer, and nitrogen inlet tube, 3-methyl-1,5-pentanediol, isophthalic acid, and plant-derived sebacic acid (manufactured by Ogura Synthetic Industries Co., Ltd.) were added together with titanium tetraisopropoxide (1,000 ppm relative to the resin component) such that the molar ratio of hydroxyl groups to carboxyl groups, [OH / COOH], was 1.1, the diol component consisted of 100 mol% 3-methyl-1,5-pentanediol, the dicarboxylic acid component consisted of 66 mol% isophthalic acid and 34 mol% sebacic acid, and the amount of trimethylolpropane in the total monomer was 1.5 mol%. The mixture was then heated to 200°C over approximately 4 hours, and then to 230°C over 2 hours, and the reaction was continued until no effluent was released. The mixture was then further reacted under reduced pressure of 10 mmHg to 15 mmHg for 5 hours to obtain [Intermediate Polyester A-1].
[0362] Next, the obtained [intermediate polyester A-1] and isophorone diisocyanate (IPDI) were added to a reaction vessel equipped with a condenser, a stirrer, and a nitrogen inlet tube in a molar ratio (isocyanate groups of IPDI / hydroxyl groups of intermediate polyester) of 2.0. After diluting with ethyl acetate to a 50% ethyl acetate solution, the mixture was reacted at 100°C for 5 hours to obtain [prepolymer A-1].
[0363] <Synthesis of amorphous polyester resin A-1> The obtained [prepolymer A-1] was stirred in a reaction vessel equipped with a heater, stirrer, and nitrogen inlet tube. Then, [ketimine compound 1] was added dropwise to the reaction vessel in an amount equal to the amount of isocyanate in [prepolymer A-1], so that the amount of amine in [ketimine compound 1] was equimolar. After stirring at 45°C for 10 hours, the prepolymer extension was removed. The obtained prepolymer extension was dried under reduced pressure at 50°C until the amount of residual ethyl acetate was 100 ppm or less to obtain [amorphous polyester resin A-1]. The physical properties of this resin are shown in Table 1 below.
[0364] (Manufacturing Example A-2: Synthesis of Amorphous Polyester Resin A-2) <Synthesis of Prepolymer A-2> In a reaction vessel equipped with a condenser, stirrer, and nitrogen inlet tube, 3-methyl-1,5-pentanediol, isophthalic acid, and plant-derived sebacic acid (manufactured by Ogura Synthetic Industries Co., Ltd.) were added together with titanium tetraisopropoxide (1,000 ppm relative to the resin component) such that the molar ratio of hydroxyl groups to carboxyl groups, [OH / COOH], was 1.1, the diol component consisted of 100 mol% 3-methyl-1,5-pentanediol, the dicarboxylic acid component consisted of 83 mol% isophthalic acid and 17 mol% sebacic acid, and the amount of trimethylolpropane in the total monomer was 1.5 mol%. The mixture was then heated to 200°C over approximately 4 hours, and then to 230°C over 2 hours, and the reaction was carried out until no more effluent water was released. The reaction was then further carried out under reduced pressure of 10 mmHg to 15 mmHg for 5 hours to obtain [intermediate polyester A-2].
[0365] Next, the obtained [intermediate polyester A-2] and isophorone diisocyanate (IPDI) were added to a reaction vessel equipped with a condenser, a stirrer, and a nitrogen inlet tube in a molar ratio (isocyanate groups of IPDI / hydroxyl groups of intermediate polyester) of 2.0. After diluting with ethyl acetate to a 50% ethyl acetate solution, the mixture was reacted at 100°C for 5 hours to obtain [prepolymer A-2].
[0366] <Synthesis of amorphous polyester resin A-2> The obtained [prepolymer A-2] was stirred in a reaction vessel equipped with a heater, stirrer, and nitrogen inlet tube. Then, [ketimine compound 1] was added dropwise to the reaction vessel in an amount that was equimolar to the amount of isocyanate in [prepolymer A-2]. After stirring at 45°C for 10 hours, the prepolymer extension was removed. The obtained prepolymer extension was dried under reduced pressure at 50°C until the amount of residual ethyl acetate was 100 ppm or less to obtain [amorphous polyester resin A-2]. The physical properties of this resin are shown in Table 1 below.
[0367] (Manufacturing Example A-3: Synthesis of Amorphous Polyester Resin A-3) <Synthesis of Prepolymer A-3> In a reaction vessel equipped with a condenser, stirrer, and nitrogen inlet, 3-methyl-1,5-pentanediol, isophthalic acid, and adipic acid were added together with titanium tetraisopropoxide (1,000 ppm relative to the resin component) such that the molar ratio of hydroxyl groups to carboxyl groups, [OH / COOH], was 1.1, the diol component consisted of 100 mol% 3-methyl-1,5-pentanediol, the dicarboxylic acid component consisted of 45 mol% isophthalic acid and 55 mol% adipic acid, and the amount of trimethylolpropane in the total monomer was 1.5 mol%. The mixture was then heated to 200°C over approximately 4 hours, and then to 230°C over 2 hours, and the reaction was continued until no effluent was released. The reaction was then carried out under reduced pressure of 10 mmHg to 15 mmHg for 5 hours to obtain [intermediate polyester A-3].
[0368] Next, the obtained [intermediate polyester A-3] and isophorone diisocyanate (IPDI) were added to a reaction vessel equipped with a condenser, a stirrer, and a nitrogen inlet tube in a molar ratio (isocyanate groups of IPDI / hydroxyl groups of intermediate polyester) of 2.0. After diluting with ethyl acetate to a 50% ethyl acetate solution, the mixture was reacted at 100°C for 5 hours to obtain [prepolymer A-3].
[0369] <Synthesis of amorphous polyester resin A-3> The obtained [prepolymer A-3] was stirred in a reaction vessel equipped with a heating device, stirrer, and nitrogen inlet tube. Then, [ketimine compound 1] was added dropwise to the reaction vessel in an amount that was equimolar to the amount of isocyanate in [prepolymer A-3]. After stirring at 45°C for 10 hours, the prepolymer extension was removed. The obtained prepolymer extension was dried under reduced pressure at 50°C until the amount of residual ethyl acetate was 100 ppm or less to obtain [amorphous polyester resin A-3]. The physical properties of this resin are shown in Table 1 below.
[0370] The amorphous polyester resin A obtained in manufacturing examples A-1 to A-3 are summarized in Table 1 below.
[0371] [Table 1]
[0372] (Manufacturing Example B-1: Synthesis of Amorphous Polyester Resin B-1) In a four-necked flask equipped with a nitrogen inlet tube, dehydration tube, stirrer, and thermocouple, plant-derived propylene glycol (Dupont), terephthalic acid, and plant-derived succinic acid (Bioamber) were charged so that the diol component consisted of 100 mol% propylene glycol, the dicarboxylic acid component consisted of 86 mol% terephthalic acid and 14 mol% succinic acid, and the molar ratio of hydroxyl groups to carboxyl groups, [OH / COOH], was 1.3. This mixture was then reacted with titanium tetraisopropoxide (500 ppm relative to the resin component) at atmospheric pressure and 230°C for 8 hours, followed by a further reaction under reduced pressure of 10 mmHg to 15 mmHg for 4 hours. After that, trimellitic anhydride was added to the reaction vessel at a concentration of 1 mol% relative to the total resin component, and the mixture was reacted at 180°C and atmospheric pressure for 3 hours to obtain [amorphous polyester resin B-1]. The physical properties of this resin are shown in Table 2 below.
[0373] (Manufacturing Example B-2: Synthesis of Amorphous Polyester Resin B-2) In a four-necked flask equipped with a nitrogen inlet tube, a dehydration tube, a stirrer, and a thermocouple, propylene glycol, bisphenol A propylene oxide 2-mol adduct, terephthalic acid, and plant-derived succinic acid (manufactured by Bioamber) were charged so that the diol component consisted of 60 mol% propylene glycol and 40 mol% bisphenol A ethylene oxide 2-mol adduct, the dicarboxylic acid component consisted of 86 mol% terephthalic acid and 14 mol% succinic acid, and the molar ratio of hydroxyl groups to carboxyl groups, [OH / COOH], was 1.3. The mixture was then reacted with titanium tetraisopropoxide (500 ppm relative to the resin component) at atmospheric pressure and 230°C for 8 hours, followed by a further reaction under reduced pressure of 10 mmHg to 15 mmHg for 4 hours. After that, trimellitic anhydride was added to the reaction vessel at a concentration of 1 mol% relative to the total resin component, and the mixture was reacted at 180°C and atmospheric pressure for 3 hours to obtain [amorphous polyester resin B-2]. The physical properties of this resin are listed in Table 2 below.
[0374] (Manufacturing Example B-3: Synthesis of Amorphous Polyester Resin B-3) In a four-necked flask equipped with a nitrogen inlet tube, dehydration tube, stirrer, and thermocouple, plant-derived propylene glycol (Dupont), terephthalic acid, and adipic acid were charged so that the diol component consisted of 100 mol% propylene glycol, the dicarboxylic acid component consisted of 97 mol% terephthalic acid and 3 mol% adipic acid, and the molar ratio of hydroxyl groups to carboxyl groups, [OH / COOH], was 1.3. This mixture was then reacted with titanium tetraisopropoxide (500 ppm relative to the resin component) at atmospheric pressure and 230°C for 8 hours, followed by a further reaction under reduced pressure of 10 mmHg to 15 mmHg for 4 hours. After that, trimellitic anhydride was added to the reaction vessel at a concentration of 1 mol% relative to the total resin component, and the mixture was reacted at 180°C and atmospheric pressure for 3 hours to obtain [amorphous polyester resin B-3]. The physical properties of this resin are shown in Table 2 below.
[0375] (Manufacturing example B-4: Synthesis of amorphous polyester resin B-4) In a four-necked flask equipped with a nitrogen inlet tube, a dehydration tube, a stirrer, and a thermocouple, bisphenol A ethylene oxide 2-mol adduct, bisphenol A propylene oxide 2-mol adduct, terephthalic acid, and adipic acid were charged so that the diol component consisted of 60 mol% bisphenol A propylene oxide 2-mol adduct and 40 mol% bisphenol A ethylene oxide 2-mol adduct, the dicarboxylic acid component consisted of 97 mol% terephthalic acid and 3 mol% adipic acid, and the molar ratio of hydroxyl groups to carboxyl groups, [OH / COOH], was 1.3. The mixture was reacted with titanium tetraisopropoxide (500 ppm relative to the resin component) at atmospheric pressure and 230°C for 8 hours, and then further reacted under reduced pressure of 10 mmHg to 15 mmHg for 4 hours. After that, trimellitic anhydride was added to the reaction vessel at a concentration of 1 mol% relative to the total resin component, and the mixture was reacted at 180°C and atmospheric pressure for 3 hours to obtain [amorphous polyester resin B-4]. The physical properties of this resin are listed in Table 2 below.
[0376] The amorphous polyester resin B obtained in manufacturing examples B-1 to B-4 are summarized in Table 2 below.
[0377] [Table 2]
[0378] (Preparation Example 1-1: Preparation of Amorphous Polyester Resin B Dispersion 1) 150 parts of [amorphous polyester resin B-1], 150 parts of methyl erketone, and 0.1 parts of sodium hydroxide (0.3N) were placed in a 500 mL separable flask and stirred with a Three-One Motor (manufactured by Shinto Kagaku Co., Ltd.) to prepare a resin mixture. While further stirring this resin mixture, 700 parts of ion-exchanged water were gradually added to induce phase inversion emulsification and desolvent removal to obtain [amorphous polyester resin B dispersion 1]. The volume-average particle size of the resin particles in the obtained [amorphous polyester resin B dispersion 1] was 50 nm, and the solid content concentration was 25%.
[0379] (Preparation Example 1-2: Preparation of Amorphous Polyester Resin B Dispersion 2) Amorphous polyester resin B dispersion 2 was obtained in the same manner as in Preparation Example 1-1, except that [amorphous polyester resin B-1] was replaced with [amorphous polyester resin B-2]. The volume-average particle size of the resin particles in the obtained Amorphous polyester resin B dispersion 2 was 62 nm, and the solid content concentration was 25%.
[0380] (Preparation Examples 1-3: Preparation of Amorphous Polyester Resin B Dispersion 3) In Preparation Example 1-1, [Amorphous Polyester Resin B Dispersion 3] was obtained using the same method as in Preparation Example 1-1, except that [Amorphous Polyester Resin B-1] was replaced with [Amorphous Polyester Resin B-3]. The volume-average particle size of the resin particles in the obtained [Amorphous Polyester Resin B Dispersion 3] was 45 nm, and the solid content concentration was 25%.
[0381] (Preparation Examples 1-4: Preparation of Amorphous Polyester Resin B Dispersion 4) In Preparation Example 1-1, [Amorphous Polyester Resin B Dispersion 4] was obtained using the same method as in Preparation Example 1-1, except that [Amorphous Polyester Resin B-1] was replaced with [Amorphous Polyester Resin B-4]. The volume-average particle size of the resin particles in the obtained [Amorphous Polyester Resin B Dispersion 4] was 40 nm, and the solid content concentration was 25%.
[0382] The amorphous polyester resin B dispersions obtained in Preparation Examples 1-1 to 1-4 are summarized in Table 3 below.
[0383] [Table 3]
[0384] (Manufacturing example C-1: Synthesis of crystalline polyester resin C-1) In a 5L four-necked flask equipped with a nitrogen inlet tube, dehydration tube, stirrer, and thermocouple, plant-derived sebacic acid (manufactured by Ogura Synthetic Industry Co., Ltd.) and 1,6-hexanediol were charged so that the molar ratio of hydroxyl groups to carboxyl groups, [OH / COOH], was 0.9. This mixture was then reacted with titanium tetraisopropoxide (500 ppm relative to the resin component) at 180°C for 10 hours, followed by a reaction at 200°C for 3 hours, and then a further reaction at a pressure of 8.3 kPa for 2 hours to obtain [crystalline polyester resin C-1]. The physical properties of this resin are shown in Table 4 below.
[0385] (Manufacturing example C-2: Synthesis of crystalline polyester resin C-2) Crystalline polyester resin C-2 was obtained in the same manner as in Production Example C-1, except that plant-derived sebacic acid as the dicarboxylic acid component was replaced with plant-derived dodecanediic acid (manufactured by Verdezyne). The physical properties of this resin are shown in Table 4 below.
[0386] (Manufacturing example C-3: Synthesis of crystalline polyester resin C-3) Crystalline polyester resin C-3 was obtained in the same manner as in Production Example C-1, except that 1,6-hexanediol as the diol component was replaced with plant-derived ethylene glycol (manufactured by India Glycols Ltd). The physical properties of this resin are shown in Table 4 below.
[0387] (Manufacturing example C-4: Synthesis of crystalline polyester resin C-4) Crystalline polyester resin C-4 was obtained in the same manner as in Production Example C-1, except that plant-derived sebacic acid as the dicarboxylic acid component was replaced with adipic acid. The physical properties of this resin are shown in Table 4 below.
[0388] The crystalline polyester resin C obtained in manufacturing examples C-1 to C-4 are summarized in Table 4 below.
[0389] [Table 4]
[0390] (Preparation Example 2-1: Preparation of crystalline polyester resin C dispersion 1) 45 parts of [crystalline polyester resin C-1] and 450 parts of ethyl acetate were placed in a container equipped with a stirring rod and thermometer. The mixture was heated to 80°C under stirring and maintained at 80°C for 5 hours. After cooling to 30°C in 1 hour, the mixture was dispersed using a bead mill (Ultraviscomill, manufactured by AIMEX) under the following conditions: liquid transfer rate of 1 kg / hour, disk peripheral speed of 6 m / second, and 80% by volume filling with 0.5 mm diameter zirconia beads, in 3 passes, to obtain [crystalline polyester resin C dispersion 1]. The volume-average particle size of the obtained crystalline polyester resin particles was 350 nm, and the solid content concentration of the resin particles was 10%.
[0391] (Preparation Example 2-2: Preparation of crystalline polyester resin C dispersion 2) In Preparation Example 2-1, [Crystalline Polyester Resin C Dispersion 2] was obtained using the same method as in Preparation Example 2-1, except that [Crystalline Polyester Resin C-1] was replaced with [Crystalline Polyester Resin C-2]. The volume-average particle size of the resin particles in the obtained [Crystalline Polyester Resin C Dispersion 2] was 350 nm, and the solid content concentration was 10%.
[0392] (Preparation Example 2-3: Preparation of crystalline polyester resin C dispersion 3) In Preparation Example 2-1, [Crystalline Polyester Resin C Dispersion 3] was obtained using the same method as in Preparation Example 2-1, except that [Crystalline Polyester Resin C-1] was replaced with [Crystalline Polyester Resin C-3]. The volume-average particle size of the resin particles in the obtained [Crystalline Polyester Resin C Dispersion 3] was 360 nm, and the solid content concentration was 10%.
[0393] (Preparation Example 2-4: Preparation of crystalline polyester resin C dispersion 4) In Preparation Example 2-1, [Crystalline Polyester Resin C Dispersion 4] was obtained using the same method as in Preparation Example 2-1, except that [Crystalline Polyester Resin C-1] was replaced with [Crystalline Polyester Resin C-4]. The volume-average particle size of the resin particles in the obtained [Crystalline Polyester Resin C Dispersion 4] was 340 nm, and the solid content concentration was 10%.
[0394] The crystalline polyester resin C dispersions obtained in Preparation Examples 2-1 to 2-4 are summarized in Table 5 below.
[0395] [Table 5]
[0396] (Preparation Example 3-1: Preparation of Masterbatch (MB)) 1,200 parts water, 500 parts carbon black (Printex35, manufactured by Dexa) [DBP oil absorption = 42 mL / 100 mg, pH = 9.5], and 500 parts [amorphous polyester resin B-1] were added and mixed in a Henschel mixer (manufactured by Nippon Coke Industries Co., Ltd.). The mixture was kneaded at 150°C for 30 minutes using two rolls, then rolled and cooled, and pulverized in a pulperizer to obtain [Masterbatch 1].
[0397] (Preparation Example 4-1: Preparation of Wax Dispersion 1) 42 parts of ester wax (WE-11, manufactured by NOF Corporation, plant-based wax, melting point 70°C) and 420 parts of ethyl acetate were charged into a container equipped with a stirring rod and thermometer. The mixture was heated to 80°C under stirring and maintained at 80°C for 5 hours, then cooled to 30°C in 1 hour. Dispersion was performed using a bead mill (UltraViscomill, manufactured by AIMEX Corporation) under the following conditions: liquid transfer rate of 1 kg / hour, disk peripheral speed of 6 m / second, and 80% by volume filling of 0.5 mm diameter zirconia beads, in 3 passes, to obtain [Wax Dispersion 1]. The volume-average particle size of the wax particles in the obtained [Wax Dispersion 1] was 420 nm, and the solid content concentration of the resin particles was 25%.
[0398] (Preparation Example 4-2: Preparation of Wax Dispersion 2) Fifty parts of paraffin wax (HNP-9, manufactured by Nippon Seiro Co., Ltd., hydrocarbon wax, melting point 75°C, SP value 8.8) and 450 parts of ethyl acetate were charged into a container equipped with a stirring rod and thermometer. The mixture was heated to 80°C under stirring and maintained at 80°C for 5 hours, then cooled to 30°C in 1 hour. Dispersion was performed using a bead mill (UltraViscomill, manufactured by AIMEX) under the following conditions: liquid transfer rate of 1 kg / hour, disk peripheral speed of 6 m / second, and 80 volume% of 0.5 mm diameter zirconia beads filled in 3 passes to obtain [Wax Dispersion 2]. The volume-average particle size of the wax particles in the obtained [Wax Dispersion 2] was 350 nm, and the solid content concentration of the resin particles was 25%.
[0399] The composition and physical properties of the wax dispersions obtained in Preparation Examples 4-1 and 4-2 are summarized in Table 6 below.
[0400] [Table 6]
[0401] (Example 1) <Preparation of the oil phase> 50 parts of [wax dispersion 1], 150 parts of [amorphous polyester resin A-1], 50 parts of [crystalline polyester resin C dispersion 1], 750 parts of [amorphous polyester resin B-1], and 50 parts of [masterbatch 1] (pigment) were placed in a container and mixed at 5,000 rpm for 60 minutes using a TK homomixer (manufactured by Primix Co., Ltd.) to obtain [oil phase 1]. The amounts of each ingredient listed represent the amount of solids in each raw material, and the same applies to the following processes.
[0402] <Preparation of the aqueous phase> 990 parts water, 20 parts sodium dodecyl sulfate, and 90 parts ethyl acetate were mixed and stirred to obtain a milky white liquid. This was designated as [Aqueous Phase 1].
[0403] <Phase inversion emulsification> [Oil phase 1] 700 parts were mixed in a TK homomixer at a rotation speed of 8,000 rpm while 20 parts of 28% ammonia water were added and mixed for 10 minutes. Then, 1,200 parts of [Aqueous phase 1] were gradually added dropwise to obtain [Emulsified slurry 1].
[0404] <Solvent removal> [Emulsified slurry 1] was placed in a container equipped with a stirrer and thermometer, and desolvented at 30°C for 180 minutes to obtain [Desolvented slurry 1]. The volume-average particle size of the particles contained in [Desolvented slurry 1] was 0.6 μm.
[0405] <Agglutination> To [Solvent-removed slurry 1], 100 parts of 3% magnesium chloride solution were added dropwise and stirred for a further 5 minutes. The temperature was then raised to 60°C, and when the particle size reached 5.0 μm, 200 parts of [Amorphous polyester resin B dispersion 4] were added dropwise and stirred for 60 minutes. Finally, 100 parts of sodium chloride were added to complete the flocculation process and obtain [Flocculated slurry 1].
[0406] <Fusion> [Agglomerated slurry 1] was heated to 70°C while stirring, and cooled when it reached the desired average circularity of 0.957 to obtain [Dispersed slurry 1].
[0407] <Washing and drying> After filtering 100 parts of [Dispersed Slurry 1] under reduced pressure, the following operations (1) to (4) were performed twice to obtain [Filtration Cake 1]. (1): 100 parts of deionized water were added to the filter cake, mixed with a TK homomixer (rotating at 12,000 rpm for 10 minutes), and then filtered. (2): 100 parts of a 10% sodium hydroxide aqueous solution were added to the filtration cake from (1) above, and the mixture was mixed in a TK homomixer (at a rotation speed of 12,000 rpm for 30 minutes), and then filtered under reduced pressure. (3): 100 parts of 10% hydrochloric acid were added to the filtered cake from (2) above, and the mixture was mixed in a TK homomixer (at a rotation speed of 12,000 rpm for 10 minutes), and then filtered. (4): 300 parts of deionized water were added to the filtration cake from (3) above, mixed with a TK homomixer (rotating at 12,000 rpm for 10 minutes), and then filtered. The obtained [filter cake 1] was dried in a circulating air dryer at 45°C for 48 hours, and then sieved with a mesh with a mesh opening of 75 μm to obtain [toner matrix particles 1].
[0408] <External additive treatment process> To 100 parts of [Toner matrix particles 1], 2.0 parts of hydrophobic silica (HDK® H2000, manufactured by Clariant Co., Ltd.) was added as an external additive and mixed in a Henschel mixer. The mixture was then passed through a 500-mesh sieve to obtain [Toner 1].
[0409] (Example 2) Toner 2 was obtained in the same manner as in Example 1, except that in the preparation of the oil phase of Example 1, [amorphous polyester resin A-1] was changed to 0 parts, [wax dispersion 1] was changed to [wax dispersion 2], and [crystalline polyester resin C dispersion 1] was changed to 80 parts.
[0410] (Example 3) Toner 3 was obtained in the same manner as in Example 1, except that in the preparation of the oil phase of Example 1, [amorphous polyester resin A-1] was changed to [amorphous polyester resin A-2], [amorphous polyester resin B-1] was changed to [amorphous polyester resin B-2], and [crystalline polyester resin C dispersion 1] was changed to [crystalline polyester resin C dispersion 4].
[0411] (Example 4) In the aggregation step of Example 1, the following steps were taken: 100 parts of [3% magnesium chloride solution] were replaced with 200 parts of [3% sodium sulfate solution], the pH was adjusted to 3 with 1% hydrochloric acid, 100 parts of [sodium chloride] were added, the pH was adjusted to 9 with 1% sodium hydroxide, and [amorphous polyester resin B dispersion 4] was replaced with [amorphous polyester resin B dispersion 1]. Otherwise, [toner 4] was obtained in the same manner as in Example 1.
[0412] (Example 5) In the preparation of the oil phase in Example 1, [amorphous polyester resin A-1] was changed to [amorphous polyester resin A-3], [amorphous polyester resin B-1] was changed to [amorphous polyester resin B-3], 50 parts of [wax dispersion 1] was changed to 200 parts, and 50 parts of [crystalline polyester resin C dispersion 1] was changed to 200 parts. In the aggregation stage, [3% magnesium chloride solution] was changed to [3% calcium chloride solution], and 200 parts of [amorphous polyester resin B dispersion 4] was changed to 230 parts of [amorphous polyester resin B dispersion 3]. In short, [toner 5] was obtained in the same manner as in Example 1.
[0413] (Example 6) In Example 1, [toner 6] was obtained in the same manner as in Example 1, except that in the <Preparation of Oil Phase>, 150 parts of [Amorphous Polyester Resin A-1] was changed to 100 parts, and [Crystalline Polyester Resin C Dispersion 1] was changed to [Crystalline Polyester Resin C Dispersion 3], and in the <Agglomeration>, 100 parts of [3% Magnesium Chloride Solution] was changed to 20 parts of [3% Aluminum Sulfate Solution], and 200 parts of [Amorphous Polyester Resin B Dispersion 4] was changed to 400 parts of [Amorphous Polyester Resin B Dispersion 2].
[0414] (Example 7) In the preparation of the oil phase in Example 1, [amorphous polyester resin A-1] was changed to [amorphous polyester resin A-3], [amorphous polyester resin B-1] was changed to [amorphous polyester resin B-3], 50 parts of [wax dispersion 1] was changed to 400 parts, and 50 parts of [crystalline polyester resin C dispersion 1] was changed to 400 parts. In the aggregation stage, 100 parts of [3% magnesium chloride solution] was changed to 200 parts of [3% sodium sulfate solution], the pH was adjusted to 3 with 1% hydrochloric acid, 100 parts of [sodium chloride] were added, the pH was adjusted to 9 with 1% sodium hydroxide, and 200 parts of [amorphous polyester resin B dispersion 4] was changed to 230 parts. Otherwise, [toner 7] was obtained in the same manner as in Example 1.
[0415] (Example 8) In Example 1, [Toner 8] was obtained in the same manner as in Example 1, except that in the <Preparation of Oil Phase>, [Crystalline Polyester Resin C Dispersion 1] was changed to [Crystalline Polyester Resin C Dispersion 3], and in the <Agglomeration>, 100 parts of [3% Magnesium Chloride Solution] was changed to 200 parts of [3% Sodium Sulfate Solution], the pH was adjusted to 3 with 1% hydrochloric acid, and after adding [100 parts of Sodium Chloride], the pH was adjusted to 9 with 1% sodium hydroxide, and 200 parts of [Amorphous Polyester Resin B Dispersion 4] was changed to 230 parts.
[0416] (Example 9) In the preparation of the oil phase in Example 1, [toner 9] was obtained in the same manner as in Example 1, except that 150 parts of [amorphous polyester resin A-1] were replaced with 50 parts of [amorphous polyester resin A-3], [amorphous polyester resin B-1] was replaced with [amorphous polyester resin B-3], 50 parts of [wax dispersion 1] were replaced with 350 parts, and 50 parts of [crystalline polyester resin C dispersion 1] were replaced with 350 parts of [crystalline polyester resin C dispersion 2].
[0417] (Example 10) In Example 1, [wax dispersion 1] was changed to [wax dispersion 2] in the <Preparation of oil phase> step, and in the <Agglomeration> step, 100 parts of [3% magnesium chloride solution] was changed to 200 parts of [3% sodium sulfate solution], the pH was adjusted to 3 with 1% hydrochloric acid, and then 100 parts of [sodium chloride] was added, followed by the adjustment to 9 with 1% sodium hydroxide, and 200 parts of [amorphous polyester resin B dispersion 4] was changed to 230 parts. Otherwise, [toner 10] was obtained in the same manner as in Example 1.
[0418] (Example 11) In the preparation of the oil phase in Example 1, [toner 11] was obtained in the same manner as in Example 1, except that 150 parts of [amorphous polyester resin A-1] was changed to 0 parts, [amorphous polyester resin B-1] was changed to [amorphous polyester resin B-2], and 50 parts of [crystalline polyester resin C dispersion 1] was changed to 200 parts of [crystalline polyester resin C dispersion 2].
[0419] (Example 12) Toner 12 was obtained in the same manner as in Example 1, except that in the preparation of the oil phase of Example 1, [amorphous polyester resin A-1] was changed to [amorphous polyester resin A-3], [amorphous polyester resin B-1] was changed to [amorphous polyester resin B-3], and [crystalline polyester resin C dispersion 1] was changed to [crystalline polyester resin C dispersion 2].
[0420] (Example 13) In the preparation of the oil phase in Example 1, [toner 13] was obtained in the same manner as in Example 1, except that 750 parts of [amorphous polyester resin B-1] were replaced with 500 parts of [amorphous polyester resin B-3], 50 parts of [wax dispersion 1] were replaced with 200 parts of [wax dispersion 2], and 50 parts of [crystalline polyester resin C dispersion 1] were replaced with 10 parts of [crystalline polyester resin C dispersion 3].
[0421] (Example 14) In Example 1, [Toner 14] was obtained in the same manner as in Example 1, except that in the <Preparation of Oil Phase>, [Amorphous Polyester Resin A-1] was changed to [Amorphous Polyester Resin A-3], [Amorphous Polyester Resin B-1] was changed to [Amorphous Polyester Resin B-3], and [Wax Dispersion 1] was changed to [Wax Dispersion 2], and in the <Agglomeration>, 200 parts of [Amorphous Polyester Resin B Dispersion 4] was changed to 400 parts.
[0422] (Example 15) In Example 1, [Toner 15] was obtained in the same manner as in Example 1, except that in the <Preparation of Oil Phase>, [Amorphous Polyester Resin B-1] was changed to [Amorphous Polyester Resin B-2], and in the <Agglomeration>, 100 parts of [3% Magnesium Chloride Solution] was changed to 200 parts of [3% Sodium Sulfate Solution], the pH was adjusted to 3 with 1% hydrochloric acid, and after adding [100 parts of Sodium Chloride], the pH was adjusted to 9 with 1% sodium hydroxide, and 200 parts of [Amorphous Polyester Resin B Dispersion 4] was changed to 400 parts.
[0423] (Example 16) In Example 1, [Toner 16] was obtained in the same manner as in Example 1, except that in the <Preparation of Oil Phase>, [Amorphous Polyester Resin A-1] was changed to [Amorphous Polyester Resin A-2], [Amorphous Polyester Resin B-1] was changed to [Amorphous Polyester Resin B-2], and [Crystalline Polyester Resin C Dispersion 1] was changed to [Crystalline Polyester Resin C Dispersion 3], and in the <Agglomeration>, 100 parts of [3% Magnesium Chloride Solution] was changed to 200 parts of [3% Sodium Sulfate Solution], the pH was adjusted to 3 with 1% hydrochloric acid, then 100 parts of [Sodium Chloride] was added, the pH was adjusted to 9 with 1% sodium hydroxide, and 200 parts of [Amorphous Polyester Resin B Dispersion 4] was changed to 400 parts.
[0424] (Example 17) In the preparation of the oil phase in Example 1, [amorphous polyester resin A-1] was changed to [amorphous polyester resin A-3], 750 parts of [amorphous polyester resin B-1] was changed to 500 parts of [amorphous polyester resin B-3], and 50 parts of [crystalline polyester resin C dispersion 1] was changed to 10 parts. In the aggregation stage, 100 parts of [3% magnesium chloride solution] was changed to 200 parts of [3% sodium sulfate solution], the pH was adjusted to 3 with 1% hydrochloric acid, 100 parts of [sodium chloride] were added, the pH was adjusted to 9 with 1% sodium hydroxide, and 200 parts of [amorphous polyester resin B dispersion 4] was changed to 400 parts. Otherwise, [toner 17] was obtained in the same manner as in Example 1.
[0425] (Example 18) In Example 1, [Toner 18] was obtained in the same manner as in Example 1, except that in the <Preparation of Oil Phase>, [Amorphous Polyester Resin A-1] was changed to [Amorphous Polyester Resin A-3], 750 parts of [Amorphous Polyester Resin B-1] was changed to 500 parts of [Amorphous Polyester Resin B-3], [Wax Dispersion 1] was changed to [Wax Dispersion 2], and [Crystalline Polyester Resin C Dispersion 1] was changed to [Crystalline Polyester Resin C Dispersion 4], and in the <Agglomeration>, 100 parts of [3% Magnesium Chloride Solution] was changed to 200 parts of [3% Sodium Sulfate Solution], the pH was adjusted to 3 with 1% hydrochloric acid, then 100 parts of [Sodium Chloride] was added, the pH was adjusted to 9 with 1% sodium hydroxide, and 200 parts of [Amorphous Polyester Resin B Dispersion 4] was changed to 400 parts.
[0426] (Comparative Example 1) [Toner 19] was obtained in the same manner as in Example 1, except that the amount of [amorphous polyester resin B dispersion 4] was changed from 200 parts to 0 parts in the <aggregation> step of Example 1.
[0427] (Comparative Example 2) In Example 1, [Toner 20] was obtained in the same manner as in Example 1, except that in the <Preparation of Oil Phase>, [Amorphous Polyester Resin A-1] was changed to [Amorphous Polyester Resin A-2], [Amorphous Polyester Resin B-1] was changed to [Amorphous Polyester Resin B-4], and [Wax Dispersion 1] was changed to [Wax Dispersion 2], and in the <Agglomeration>, 100 parts of [3% Magnesium Chloride Solution] was changed to 200 parts of [3% Sodium Sulfate Solution], the pH was adjusted to 3 with 1% hydrochloric acid, and after adding [100 parts of Sodium Chloride], the pH was adjusted to 9 with 1% sodium hydroxide, and 200 parts of [Amorphous Polyester Resin B Dispersion 4] was changed to 50 parts.
[0428] (Comparative Example 3) In Example 1, [Toner 21] was obtained in the same manner as in Example 1, except that in the <Preparation of Oil Phase>, [Amorphous Polyester Resin A-1] was changed to [Amorphous Polyester Resin A-3], [Amorphous Polyester Resin B-1] was changed to [Amorphous Polyester Resin B-4], and [Wax Dispersion 1] was changed to [Wax Dispersion 2], and in the <Agglomeration>, 200 parts of [Amorphous Polyester Resin B Dispersion 4] was changed to 400 parts.
[0429] (Comparative Example 4) In the preparation of the oil phase in Example 1, [amorphous polyester resin A-1] was changed to [amorphous polyester resin A-3], [amorphous polyester resin B-1] was changed to [amorphous polyester resin B-4], [wax dispersion 1] was changed to [wax dispersion 2], and [crystalline polyester resin C dispersion 1] was changed to [crystalline polyester resin C dispersion 3]. In the aggregation stage, 200 parts of [amorphous polyester resin B dispersion 4] was changed to 0 parts. In short, [toner 22] was obtained in the same manner as in Example 1.
[0430] (Comparative Example 5) In Example 1, [Toner 23] was obtained in the same manner as in Example 1, except that in the <Preparation of Oil Phase>, [Amorphous Polyester Resin A-1] was changed to [Amorphous Polyester Resin A-3], [Amorphous Polyester Resin B-1] was changed to [Amorphous Polyester Resin B-4], and [Wax Dispersion 1] was changed to [Wax Dispersion 2], and in the <Agglomeration>, 100 parts of [3% Magnesium Chloride Solution] was changed to 200 parts of [3% Sodium Sulfate Solution], the operation of adjusting the pH to 3 with 1% hydrochloric acid was added, followed by the addition of [100 parts of Sodium Chloride], then the operation of adjusting the pH to 9 with 1% sodium hydroxide, and 200 parts of [Amorphous Polyester Resin B Dispersion 4] was changed to 50 parts.
[0431] (Comparative Example 6) In Example 1, the preparation of the oil phase was changed from 150 parts to 50 parts of [amorphous polyester resin A-1], [amorphous polyester resin B-1] was changed to [amorphous polyester resin B-4], and [crystalline polyester resin C dispersion 1] was changed to [crystalline polyester resin C dispersion 3]. In the aggregation stage, 100 parts of [3% magnesium chloride solution] was changed to 200 parts of [3% sodium sulfate solution], the pH was adjusted to 3 with 1% hydrochloric acid, 100 parts of [sodium chloride] were added, the pH was adjusted to 9 with 1% sodium hydroxide, and 200 parts of [amorphous polyester resin B dispersion 4] was changed to 50 parts of [amorphous polyester resin B dispersion 3]. Otherwise, [toner 24] was obtained in the same manner as in Example 1.
[0432] (Comparative Example 7) In the preparation of the oil phase in Example 1, [amorphous polyester resin A-1] was changed to [amorphous polyester resin A-3], [wax dispersion 1] was changed to [wax dispersion 2], and [crystalline polyester resin C dispersion 1] was changed to [crystalline polyester resin C dispersion 4]. In the aggregation stage, 200 parts of [amorphous polyester resin B dispersion 4] were changed to 0 parts. In short, [toner 25] was obtained in the same manner as in Example 1.
[0433] (Comparative Example 8) In the preparation of the oil phase in Example 1, [amorphous polyester resin A-1] was changed to [amorphous polyester resin A-3], [amorphous polyester resin B-1] was changed to [amorphous polyester resin B-3], [wax dispersion 1] was changed to [wax dispersion 2], and [crystalline polyester resin C dispersion 1] was changed to [crystalline polyester resin C dispersion 4]. In the aggregation stage, 200 parts of [amorphous polyester resin B dispersion 4] was changed to 0 parts. In short, [toner 26] was obtained in the same manner as in Example 1.
[0434] (Comparative Example 9) In Example 1, the preparation of the oil phase was changed from 150 parts of [amorphous polyester resin A-1] to 0 parts, [amorphous polyester resin B-1] to [amorphous polyester resin B-4], [wax dispersion 1] to [wax dispersion 2], and [crystalline polyester resin C dispersion 1] to [crystalline polyester resin C dispersion 2]. In addition, in the aggregation stage, the toner 27 was obtained in the same manner as in Example 1, except that 200 parts of [amorphous polyester resin B dispersion 4] were changed to 400 parts.
[0435] (Comparative Example 10) In Example 1, the preparation of the oil phase was changed from 150 parts of amorphous polyester resin A-1 to 50 parts of amorphous polyester resin A-2, from amorphous polyester resin B-1 to amorphous polyester resin B-2, and from crystalline polyester resin C dispersion 1 to crystalline polyester resin C dispersion 2. In addition, in the coagulation step, 100 parts of 3% magnesium chloride solution was changed to 200 parts of 3% sodium sulfate solution, the pH was adjusted to 3 with 1% hydrochloric acid, 100 parts of sodium chloride were added, the pH was adjusted to 9 with 1% sodium hydroxide, and 200 parts of amorphous polyester resin B dispersion 4 were changed to 0 parts. Otherwise, toner 28 was obtained in the same manner as in Example 1.
[0436] The composition of the oil phase components in Examples 1 to 18 and Comparative Examples 1 to 10, as well as the characteristics of the aggregation, phase inversion emulsification, and solvent removal processes, are shown in Tables 7-1 to 7-5 below.
[0437] [Table 7-1]
[0438] [Table 7-2]
[0439] [Table 7-3]
[0440] [Table 7-4]
[0441] [Table 7-5]
[0442] For each toner obtained in Examples 1-18 and Comparative Examples 1-10, the following method was used to determine the proportion of crystalline polyester resin C in the region within 150 nm from the outermost surface of the toner particles (hereinafter sometimes referred to as "proportion of crystalline polyester near the surface") and the radioactive isotope indicating the plant content. 14 The C concentration, THF-insoluble content (gel content), domain length of crystalline polyester C, and aspect ratio of crystalline polyester C were measured. The results are shown in Tables 8-1 and 8-2 below.
[0443] <Measurement of the proportion of the crystalline resin in the region within 150 nm from the outermost surface of the resin particles> The proportion of the crystalline polyester resin C in the region within 150 nm from the outermost surface of each toner (the proportion of crystalline polyester near the surface) was measured by the following method. Each toner sample was embedded in epoxy resin (S-31, manufactured by DEVCON), cut to a thickness of 60 nm using an ultrasonic ultramicrotome (Leica EM UC7, manufactured by Leica), and stained with ruthenium (RuO4) using a vacuum staining device (Filgen Co., Ltd.). Subsequently, the toner cross-sections were observed using a transmission electron microscope (H-7500, manufactured by Hitachi High-Tech Corporation) at an acceleration voltage of 120 kV. For this observation, 50 toner samples were arbitrarily selected from those with a particle size within ±2.0 μm of the weight-average particle size of the toner sample and photographed.
[0444] The proportion of crystalline resin in the region within 150 nm from the outermost surface of each toner was calculated using image processing software (Image-J) as follows. (1) The outer periphery of all crystalline polyester resin C domains that are unevenly distributed in the cross-sectional image of one toner was enclosed with freehand sections, and the area was measured using Analyze, and the sum of these was defined as "Area A". (2) The outer circumference of a single toner particle in the cross-sectional image was enclosed with freehand sections to create "Region 1". (3) The center of mass of "Region 1" was determined by Analyze. (4) Using a proprietary plugin, a "region 2" was created by taking 100 points at a distance of 150 nm from the center of gravity of the toner particle determined in (3) from the coordinates obtained by dividing the outer perimeter of "region 1," that is, the line that encloses the outer perimeter of one toner particle in (2) with Freehand-sections into 100 equally spaced points, and connecting these points with straight lines. (5) "Region 3" was created by subtracting "Region 2" created in (4) from "Region 1" created in (2). (6) The outer periphery of the crystalline polyester resin C domain present in "Region 3" created in (5) above was enclosed with Freehand sections, the area was measured using Analyze, and the sum of these areas was defined as "Area B". (7) By substituting the "area A" calculated in (1) above and the "area B" calculated in (6) above into the following equation (2), the proportion of crystalline polyester resin C in the region within 150 nm from the outermost surface of a single toner particle was calculated. The percentage of crystalline polyester resin C within 150 nm from the outermost surface of a single resin particle [%] = Area A / Area B × 100 ... Equation (2) (8) The operations described in (1) to (7) above were performed on 50 toner particles, and the average value of the proportion of crystalline polyester resin C in the region within 150 nm from the outermost surface of the 50 toner particles was calculated. This average value was taken as the proportion of crystalline polyester resin C in the region within 150 nm from the outermost surface of the toner particles.
[0445] <Radioisotope 14 Measurement of C concentration > Radiocarbon isotopes of each toner14 The C concentration was measured by radiocarbon dating. The toner was combusted to reduce its CO2 (carbon dioxide) to obtain C (graphite). Of the C (graphite) 14 the C concentration was measured using an accelerator mass spectrometer (AMS, manufactured by Beta Analytic Inc.). An oxalic acid standard (HOxII, manufactured by NIST) was used as the standard sample.
[0446] <Measurement of THF-insoluble content (gel content)> The THF-insoluble content of each toner was measured as follows. 1 part of toner was added to 100 parts of tetrahydrofuran (THF), and after refluxing for 6 hours, the insoluble component was precipitated by a centrifuge to separate the insoluble component from the supernatant. The mass of the insoluble component dried at 40°C for 20 hours was divided by the mass of the initially used toner, and the result was multiplied by 100 to calculate the content of the THF-insoluble fraction.
[0447] <Measurement of average major axis diameter and average aspect ratio of crystalline polyester> The average major axis diameter and average aspect ratio of the crystalline polyester resin C in each toner were measured by the following method. The toner was embedded in an epoxy resin (S-31, manufactured by DEVCON), cut to a thickness of 60 nm with an ultrasonic ultramicrotome (Leica EM UC7, manufactured by Leica), and subjected to ruthenium staining (RuO4 staining) using a vacuum staining apparatus (manufactured by Filgen Inc.). Thereafter, the cross section of the toner was observed with a transmission electron microscope (H-7500, manufactured by Hitachi High-Technologies Corporation) at an acceleration voltage of 120 kV. At this time, 50 toners to be observed were arbitrarily selected from those within ±2.0 μm of the weight average particle diameter of the resin particles, and photographed.
[0448] The major axis diameter and aspect ratio of the crystalline polyester resin C in each toner were calculated as follows using image processing software (Image-Pro Plus 5.1). (1) Cross-sectional images of toner particles taken using the method described above were used. First, in order to extract the toner particles to be analyzed, the toner particle portion was selected to separate the toner particles from the background. (2) Select "Measurement" - "Count / Size" in Image-Pro Plus 5.1. From the "Count / Size" window, select "Measurement" - "Measurement Item". From the measurement items, select "Diameter (Minimum)" and "Diameter (Maximum)". In "Brightness Range Selection", adjust the brightness range so that only the crystalline polyester resin C in one of the resin particles selected in (1) above is selected. Select "Count" to display the measurement results. (3) The "maximum diameter" obtained in (2) above was taken as the major axis of the crystalline polyester resin C. The "minimum diameter" obtained in (2) above was taken as the minor axis, and the "maximum diameter" was taken as the major axis, and the aspect ratio (major axis / minor axis) of the crystalline polyester resin C was determined. (4) From the data on the major axis and aspect ratio of each crystalline polyester resin C in a single toner particle obtained in (1) to (3) above, the average value of 10 points was calculated in descending order of "diameter (maximum)". (5) The operations described in (1) to (4) above were repeated for 50 toner particles to calculate the average major axis and aspect ratio of the 50 resin particles, and this average value was taken as the average major axis and average aspect ratio of the crystalline polyester resin C in the toner particles.
[0449] [Table 8-1]
[0450] [Table 8-2]
[0451] Furthermore, carbon neutrality, filming resistance, and low-temperature fixing properties were evaluated for each toner obtained in Examples 1-18 and Comparative Examples 1-10 using the following methods. The results are shown in Tables 9-1 and 9-2 below.
[0452] <Evaluation Method> <<Carbon Neutrality>> Radioactive isotopes of toner 14 Based on the C concentration, "carbon neutrality" was evaluated according to the following evaluation criteria. - Evaluation Criteria for "Carbon Neutrality" - ◎: 35.0 pMC or higher ○: 20.0 pMC or higher, less than 35.0 pMC △: 5.4 pMC or higher and less than 20.0 pMC ×: Less than 5.4 pMC
[0453] <<Filming resistance>> A developer was obtained by mixing the carrier used in the imagio MP C5503 (manufactured by Ricoh Co., Ltd.) with the toners obtained in Examples 1-18 and Comparative Examples 1-10, so that the toner concentration was 5% by mass. After adding the developer to the imagio MP C5503 unit (manufactured by Ricoh Co., Ltd.), the amount of adhesion was 0.4 mg / cm². 2 The solid image was printed onto paper (Ricoh Type6200, A4 size) through exposure, development, and transfer processes, and a continuous paper-feed test of 2,000 sheets was conducted. Contamination of the latent image carrier (photoreceptor) and the contamination status were visually observed using a charging device, and "filming resistance" was evaluated based on the following evaluation criteria. - Evaluation criteria for "filming resistance" - ◎: No contamination on the latent image carrier and no filming on the charging device. ○: Contamination on the latent image carrier and slight filming on the charging device. △: There is slight contamination on the latent image carrier and some filming on the charging device, which may cause abnormal images to appear over time. ×: Contamination of the latent image carrier and slight filming on the charging device resulted in the early occurrence of abnormal images.
[0454] <<Low Temperature Fixation>> A developer was obtained by mixing the carrier used in the imagio MP C5503 (manufactured by Ricoh Co., Ltd.) with the toners obtained in Examples 1-18 and Comparative Examples 1-10, so that the toner concentration was 5% by mass. After adding the developer to the imagio MP C5503 unit (manufactured by Ricoh Co., Ltd.), a 2cm x 15cm rectangular solid image was printed on PPC paper type 6000 <70W> A4 T-grain (manufactured by Ricoh Co., Ltd.) with a toner adhesion rate of 0.40 mg / cm². 2 The image was formed in such a manner. At this time, the surface temperature of the fixing roller was changed, and it was observed whether a cold offset occurred in which the remaining image of the solid color was fixed to a location other than the desired location. The cold offset temperature (lower fixing limit temperature) was determined, and the "low-temperature fixing performance" was evaluated based on the evaluation criteria below. - Evaluation criteria for "low-temperature fixation" - ◎: Cold offset temperature is less than 110℃ ○: Cold offset temperature is 110°C or higher and less than 120°C △: Cold offset temperature is between 120°C and 130°C. ×: Cold offset temperature is 130°C or higher
[0455] [Table 9-1]
[0456] [Table 9-2]
[0457] Examples of embodiments of the present invention include the following: <1> Resin particles containing at least a binder resin, The aforementioned binder resin consists of an amorphous polyester resin and a crystalline resin. The alcohol monomer of the amorphous polyester resin contains propylene glycol, The proportion of the crystalline resin in the region within 150 nm from the outermost surface of the resin particles is 4% or less of the total amount of the resin particles. Radiocarbon isotopes 14 These resin particles are characterized by having a C concentration of 5.4 pMC or higher. <2> Radiocarbon isotopes 14 The C concentration is 20.0 pMC or higher. <1> These are the resin particles described in [the document]. <3> Radiocarbon isotopes 14 The C concentration is 35.0 pMC or higher. <1> from <2> These are resin particles as described in any of the following. <4> The resin particles have an insoluble content in tetrahydrofuran of 20% by mass or more. <1> from <3> These are resin particles as described in any of the following. <5> The acid component of the amorphous polyester resin contains at least one of succinic acid and sebacic acid. <1> from <4> These are resin particles as described in any of the following. <6> The major axis of the domains of the crystalline resin in the resin particles is 500 nm or less. The aspect ratio (major axis / minor axis) of the domain is 4.0 or greater. <1> from <5> These are resin particles as described in any of the following. <7> The acid component of the crystalline resin contains sebaciic acid. <6> These are the resin particles described in [the document]. <8> The aforementioned <1> from <7> These are resin particles for toner, characterized by containing resin particles as described in any of the above. <9> The aforementioned <8> This toner is characterized by containing the resin particles for toner described in [the relevant document]. <10> Furthermore, the above contains an external additive. <9> This is the toner described in [the document]. <11> The aforementioned <1> from <7> A method for producing resin particles as described in any of the following: a) A step of preparing an oil phase in which at least a crystalline resin and an amorphous polyester resin are dissolved or dispersed in an organic solvent, b) A step of adding an aqueous medium to the oil phase to convert the water-in-oil dispersion to an oil-in-water dispersion, c) A step of obtaining aggregated particles by agglomerating the particles of the oil-in-water dispersion, and then adding an amorphous polyester resin to obtain resin particles, Includes, The alcohol monomer of the amorphous polyester resin contains propylene glycol, The proportion of the crystalline resin in the region within 150 nm from the outermost surface of the resin particles is 4% or less of the total amount of the resin particles. Radioactive carbon isotopes of the aforementioned resin particles 14 This is a method for producing resin particles, characterized in that the C concentration is 5.4 pMC or higher. <12> The aforementioned <8> This is a method for producing toner, characterized by adding an external additive to the toner resin particles described above. <13> The aforementioned <9> from <10> This developer is characterized by containing the toner described in any of the following. <14> The aforementioned <9> from <10> This toner storage unit is characterized by containing toner as described in any of the above. <15> Electrostatic latent image carrier, An electrostatic latent image forming means for forming an electrostatic latent image on the electrostatic latent image carrier, A developing means comprising a toner that develops the electrostatic latent image formed on the electrostatic latent image carrier to form a visible image, It has, The toner, <9> from <10> This is an image forming apparatus characterized by using a toner as described in any of the following. <16> A step of forming an electrostatic latent image on the electrostatic latent image carrier, A developing step comprising a toner that develops the electrostatic latent image formed on the electrostatic latent image carrier using the toner to form a visible image, Includes, The toner, <9> from <10> This is an image forming method characterized by using a toner as described in any of the above.
[0458] The aforementioned <1> from <7> Resin particles as described in any of the above <8> The resin particles for toner described above, <9> from <10> Toner as described in any of the above <11> The method for producing resin particles as described above <12> The method for manufacturing toner described above <13> The developer described above, <14> The toner storage unit described above, <15> The image forming apparatus described above, and the <16> The image forming method described above can solve the aforementioned problems of the conventional method and achieve the objectives of the present invention. [Explanation of symbols]
[0459] 1. Resin particles 2. Domains derived from crystalline resins 3 Domains derived from amorphous resins 10. Photoconductor (photoconductor drum, electrostatic latent image carrier) Electrostatic latent image carrier for 10K black Electrostatic latent image carrier for 10Y yellow 10M Magenta Electrostatic Latent Image Carrier 10C Cyan Electrostatic Latent Image Carrier 14 Support rollers 15 Support rollers 16 Support rollers 17 Intermediate Transfer Body Cleaning Apparatus 18 Image forming means 20. Charging device (charging roller) 21 Exposure apparatus 22 Secondary transfer device 23 Laura 24 Secondary transfer belt 25 Fixing device 26 Fixing belt 27 Pressure roller 28 Sheet reversing device 30 Exposure apparatus 32 Contact Glasses 33 First running unit 34 Second running unit 35. Imaging lens 36 Reading Sensor 40 Developer 41 Developing belt 42K Developer Storage Section 42Y Developer storage section 42M Developer storage section 42C Developer storage section 43K Developer supply roller 43Y Developer supply roller 43M Developer supply roller 43C Developer supply roller 44K developing roller 44Y Developing Roller 44M developing roller 44C Developing Roller 45K Black Developer Unit 45Y Yellow Developer Unit 45M Magenta Developer Unit 45C Cyan Developer Unit 49 Registrola 50 Intermediate Transfer 51 Laura 52 Separation Roller 53 Manual feed path 54 Manual feed tray 55 Switching claw 56 Discharge roller 57 Paper output tray 58 Corona Charger 60 Cleaning device 61 Developing device 62 Transfer Charger 63 Photoconductor Cleaning Device 64 Static eliminator 70 Static electricity removal lamp 80 Transfer Rollers 90 Cleaning device 95 Transfer paper 100A, 100B, 100C image forming device 110 Process Cartridges 120 Tandem Developer 130 Manuscript Stand 142 Paper feed roller 143 Paper Bank 144 Paper feed cassette 145 Separation Roller 146 Paper feed path 147 Conveyor rollers 148 Paper feed path 150 Copying device main unit 160 Charging device 200 Paper feed table 300 Scanners 400 Automatic Document Feeder (ADF) L exposure [Prior art documents] [Patent Documents]
[0460] [Patent Document 1] Japanese Patent Publication No. 2015-102842
Claims
1. Resin particles containing at least a binder resin, The aforementioned binder resin consists of an amorphous polyester resin and a crystalline resin. The alcohol monomer of the amorphous polyester resin contains propylene glycol, The amorphous polyester resin contains an amorphous polyester resin having a glass transition temperature of -60°C or higher and 20°C or lower. The proportion of the crystalline resin in the region within 150 nm from the outermost surface of the resin particles is 4% or less of the total amount of the resin particles. Radiocarbon isotopes 14 Resin particles characterized by having a C concentration of 5.4 pMC or higher.
2. Radiocarbon isotopes 14 The resin particles according to claim 1, wherein the C concentration is 20.0 pMC or more.
3. Radiocarbon isotopes 14 The resin particles according to claim 1, wherein the C concentration is 35.0 pMC or higher.
4. The resin particles according to claim 1, wherein the insoluble content of the resin particles in tetrahydrofuran is 20% by mass or more.
5. The resin particles according to claim 1, wherein the acid component of the amorphous polyester resin contains at least one of succinic acid and sebacic acid.
6. The major axis of the domains of the crystalline resin in the resin particles is 500 nm or less. The resin particle according to claim 1, wherein the aspect ratio (major axis / minor axis) of the domain is 4.0 or greater.
7. The resin particles according to claim 6, wherein the acid component of the crystalline resin contains sebaciic acid.
8. Toner resin particles characterized by containing the resin particles described in claim 1.
9. A toner characterized by containing the resin particles for toner described in claim 8.
10. The toner according to claim 9, further containing an external additive.
11. A method for producing resin particles according to claim 1, a) A step of preparing an oil phase in which at least a crystalline resin and an amorphous polyester resin are dissolved or dispersed in an organic solvent, b) A step of adding an aqueous medium to the oil phase to convert the water-in-oil dispersion to an oil-in-water dispersion, c) A step of obtaining aggregated particles by agglomerating the particles of the oil-in-water dispersion, and then adding an amorphous polyester resin to obtain resin particles, Includes, The alcohol monomer of the amorphous polyester resin contains propylene glycol, The proportion of the crystalline resin in the region within 150 nm from the outermost surface of the resin particles is 4% or less of the total amount of the resin particles. Radioactive carbon isotopes of the aforementioned resin particles 14 A method for producing resin particles, characterized in that the C concentration is 5.4 pMC or higher.
12. A method for producing toner, characterized by adding an external additive to the toner resin particles described in claim 8.
13. A developer characterized by containing the toner described in claim 9.
14. A toner storage unit characterized by storing the toner described in claim 9.
15. Electrostatic latent image carrier, An electrostatic latent image forming means for forming an electrostatic latent image on the electrostatic latent image carrier, A developing means comprising a toner that develops the electrostatic latent image formed on the electrostatic latent image carrier to form a visible image, It has, An image forming apparatus characterized in that the toner is the toner described in claim 9.
Citation Information
Patent Citations
Rosin resin and toner containing rosin resin
JP2012149254A
Toner
JP2015102842A
Image forming method
JP2016040573A
Toner
JP2021047401A
Toner for electrostatic charge image development
JP2021148894A