Translucent paper and method for manufacturing translucent paper
A translucent paper with specific base paper composition and transparent material application addresses strength and recyclability challenges, ensuring high transparency and recyclability for packaging and printing applications.
Patent Information
- Application Number
- JP2022185091
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-11-18
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2042-11-18
AI Technical Summary
Existing translucent papers, such as glassine paper, lack sufficient strength for packaging applications and have issues with recyclability due to the presence of transparent resin, which affects disintegration properties during recycling.
A translucent paper is produced with a base paper composition of 30-100 g/m² basis weight, 10-70 g/m² coating/impregnation of a transparent material, and a C/(W+C) ratio of 20-40%, using coniferous and hardwood chemical pulps, with a refractive index of 1.4 to 1.6, to achieve transparency and recyclability.
The paper achieves high transparency and recyclability, suitable for packaging and printing, with improved visibility and reduced light scattering, while maintaining paper strength and preventing resin-related disintegration issues.
Smart Images

Figure 0007947932000004 
Figure 0007947932000005 
Figure 0007947932000006
Abstract
Description
[Technical Field]
[0001] This invention relates to translucent paper and a method for manufacturing translucent paper. More specifically, it relates to translucent paper that can be used as packaging paper, printing paper, publishing paper, information paper, etc., and in which a portion or the entire area of the paper is translucent, and a method for manufacturing translucent paper. [Background technology]
[0002] Paper packaging such as envelopes and product packaging may have a window that allows the recipient's address and contents to be seen from the outside. This window may be covered with a transparent resin film or glassine paper. From the perspective of resource recycling, it is preferable to use the latter, glassine paper.
[0003] Glassine paper is a translucent paper that has been conventionally known, produced by finely beating pulp to make paper and then calendering it under high pressure. However, glassine paper lacks sufficient strength for use as packaging material such as envelopes, and its applications have been limited, such as being applied only to the window of an envelope. As an alternative to glassine paper, a method has been proposed in which a transparent resin is impregnated between the fibers of the paper (for example, Patent Documents 1-4). By impregnating the voids between the cellulose fibers of the paper with a transparent resin, the transparency of the translucent areas impregnated with the transparent resin can be increased. Since translucent paper has superior strength compared to glassine paper, it can be used as packaging material such as envelopes. [Prior art documents] [Patent Documents]
[0004] [Patent Document 1] Japanese Unexamined Patent Publication No. 132698 / 1983 [Patent Document 2] Japanese Patent Publication No. 132699 / 1983 [Patent Document 3] Japanese Patent Publication No. 2018-9047 [Patent Document 4] Japanese Patent Publication No. 2021-91481 [Overview of the project] [Problems that the invention aims to solve]
[0005] However, it contains a transparent resin. Soaking The resulting translucent paper is highly transparent, but it has been found that this affects its disintegration properties when recycled as waste paper pulp after use. This invention contains a transparent resin. Soaking This invention provides translucent paper and a method for manufacturing translucent paper that achieve both transparency and recyclability. [Means for solving the problem]
[0006] The present invention has the following aspects. [1] A base paper for translucent paper, and a transparent material applied to at least a portion of the base paper for translucent paper. Soaking A translucent paper having a translucent region, characterized in that it satisfies all of the following requirements (1) to (3). Requirement (1): The basis weight (W) of the base paper for translucent paper is 30-100 g / m². 2 Requirement (2): Coating / containment per unit area of the translucent region Soaking Quantity (C) is 10-70g / m 2 Requirement (3): The value of C / (W+C)×100 is 20-40% [2] The translucent paper described in [1], wherein the base paper for translucent paper is mainly composed of coniferous chemical pulp and hardwood chemical pulp. [3] The translucent paper described in [2], wherein the ratio of coniferous chemical pulp to hardwood chemical pulp is 80:20 to 51:49. [4] The translucent paper described in [1], wherein the refractive index of the transparency material is 1.4 to 1.6.
[0007] [5] The translucent paper described in [1] wherein the translucent region has a luminous transmittance (T50) of 20% or more under the measurement condition 1 below. "Measurement Condition 1" Using a luminous transmittance meter with a gap of at least 50 mm between the light-emitting and light-receiving sections, A sample for measuring the translucent region of the translucent paper, Luminous transmittance (T50) when measured by placing one side of the sample in contact with the light projecting unit.
[0008] [6] The translucent paper according to [1] or [5], wherein the translucent region has a luminous transmittance ratio of 44 or more under Measurement Condition 2 below. "Measurement Condition 2" Using a luminous transmittance measuring instrument with a distance of at least 50 mm between the light projecting unit and the light receiving unit, A sample for measuring the translucent region of the paper is used, Measure the luminous transmittance (T50) when measured by placing one side of the sample in contact with the light projecting unit, and the luminous transmittance (T0) when measured by placing the other side of the sample in contact with the light receiving unit, and determine the luminous transmittance ratio by the following formula. Formula 1: Luminous transmittance ratio = (T50 / T0) × 100
[0009] [7] A method for producing translucent paper, wherein a coating and impregnating liquid containing a clarifying material is applied to and / or impregnated into at least a partial region of base paper for translucent paper Soaking the liquid is applied and / or impregnated Soaking to form a translucent region, the method for producing translucent paper satisfying all of the following requirements (1) to (3). Requirement (1): The basis weight (W) of the base paper for translucent paper is 30 to 100 g / m 2 Requirement (2): The coating and impregnating amount (C) per unit area of the translucent region is 10 to 70 g / m Soaking amount (C) is 10 to 70 g / m 2 Requirement (3): The value of C / (W+C)×100 is 20 to 40%. [8] The translucent paper according to [7], wherein the base paper for translucent paper is mainly composed of softwood chemical pulp and hardwood chemical pulp. [9] The translucent paper according to [8], wherein the ratio of softwood chemical pulp to hardwood chemical pulp is 80:20 to 51:49.
[10] The Canadian Standard Freeness of the softwood chemical pulp is 400 to 700 mL, and the Canadian Standard Freeness of the hardwood chemical pulp is 350 to 650 mL. A method for producing translucent paper as described in [8] or [9]. [Effects of the Invention]
[0010] The present invention provides a translucent paper that is highly transparent and recyclable, and a method for producing the translucent paper. [Brief explanation of the drawing]
[0011] [Figure 1] This is a schematic plan view illustrating an example of translucent paper. [Figure 2] This figure schematically shows the II cross-section of the translucent paper shown in Figure 1. [Figure 3] This figure schematically shows a cross-section II of the translucent paper in another embodiment of Figure 1. [Figure 4] This is an explanatory diagram illustrating the excellent visibility provided by transparent resin film. [Figure 5] This is an explanatory diagram illustrating the insufficient visibility of conventional semi-transparent paper and similar materials. [Figure 6] This is a schematic diagram illustrating an example of a method for measuring luminous transmittance. [Figure 7] This is a schematic diagram illustrating an example of a method for measuring luminous transmittance ratio. [Modes for carrying out the invention]
[0012] (translucent paper) The translucent paper of the present invention is made by applying a transparency material to at least a portion of the base paper for translucent paper. Soaking By doing so, application and inclusion Soaking The area becomes semi-transparent, resulting in semi-transparent paper. Soaking This can be applied to the entire surface of the translucent paper base when viewed from above, or to only a portion of it. There are no particular limitations on the shape or number of these areas. (Application / Containment of transparency material) SoakingIn the treated region, the clarifying material penetrates in the thickness direction of the base paper for translucent paper, and the voids inside the paper are filled with the clarifying material as much as possible, whereby the paper becomes translucent. The term "translucent treatment" means that the opacity of the paper after treatment is lower than the opacity of the paper before treatment, and is not particularly limited, but "translucent" means that the opacity of the treated region is about 4 to 25%.
[0013] Further, the translucent paper of the present invention needs to satisfy all of the following requirements (1) to (3). Requirement (1): The basis weight (W) of the base paper for translucent paper is 30 to 100 g / m 2 Requirement (2): Coating and impregna- per unit area of the translucent region Soaking tion amount (C) is 10 to 70 g / m 2 Requirement (3): The value of C / (W+C)×100 is 20 to 40%
[0014] Requirement (1): The basis weight (W) of the base paper for translucent paper is 30 to 100 g / m 2 The basis weight is preferably 40 to 80 g / m 2 , more preferably 43 to 70 g / m 2 , even more preferably 45 to 65 g / m 2 . When the basis weight is at least the lower limit of the above numerical range, the strength of the paper can be obtained, and the translucent paper is suitable for applications such as packaging paper and printing paper. When the basis weight is at most the upper limit of the above numerical range, the transparency of the translucent paper can be enhanced. The basis weight is measured in accordance with JIS P8124.
[0015] Requirement (2): Coating and impregna- per unit area of the translucent region Soaking tion amount (C) is 10 to 70 g / m 2 . The coating and impregna- Soaking tion amount is more preferably 20 to 60 g / m 2 , still more preferably 25 to 60 g / m 2This is even more preferable. If the coating / impregnation amount per unit area is greater than or equal to the lower limit of the above numerical range, the transparency of the translucent region is easily enhanced. If the coating / impregnation amount per unit area is less than or equal to the upper limit of the above numerical range, the recyclability can be enhanced. Here, the coating / impregnation amount per unit area of the translucent region Soaking Quantity refers to the amount applied to or contained in this area. Soaking This refers to the mass of the solid components, including not only the transparent material that has penetrated into the paper, but also the transparent material that is attached to the surface of the paper, or the coating / containment. Soaking This is the solid content mass of the material after drying, including the added additives.
[0016] Requirement (3): Furthermore, coating / containing Soaking When the quantity is C and the basis weight is W, the value of C / (W+C)×100 needs to be between 20% and 40%. Preferably, it is between 25% and 38%, and more preferably between 28% and 36%. If this value is above the lower limit of the above numerical range, the transparency of the translucent area can be easily increased, and if it is below the upper limit of the above numerical range, the recyclability can be improved.
[0017] The translucent paper of the present invention is made by coating a translucent material onto a base paper for translucent paper as described above. Soaking This results in a paper in which the area into which the transparent material has permeated becomes semi-transparent. For example, as shown in Figure 1, the semi-transparent area 4 may be formed in a portion of the planar view of the base paper 2 for semi-transparent paper. For example, this includes semi-transparent paper 1A, which has a base paper 2 for semi-transparent paper and a semi-transparent area 4 in which the transparent material 3 is impregnated within the base paper 2, as illustrated in Figures 1 and 2, and semi-transparent paper 1B, which has a base paper 2 for semi-transparent paper and a semi-transparent area 4 in which the transparent material 3 is impregnated within the base paper 2 and a coating layer 5 covering the semi-transparent area 4, as illustrated in Figures 1 and 3. When there is a coating layer 5, the coating and impregnation per unit area of the semi-transparent area Soaking In terms of quantity, application of the coating layer, Soaking Include the quantity.
[0018] (Translucent paper base paper) The base paper for translucent paper is not particularly limited, but it is preferably paper mainly composed of coniferous chemical pulp and hardwood chemical pulp. Examples of coniferous chemical pulp include unbleached coniferous kraft pulp (NUKP), bleached coniferous kraft pulp (NBKP), semi-bleached coniferous kraft pulp (NSBKP), unbleached coniferous sulfite pulp (NUSP), bleached coniferous sulfite pulp (NBSP), and semi-bleached coniferous sulfite pulp (NSBSP). Examples of hardwood chemical pulp include unbleached hardwood kraft pulp (LUKP), bleached hardwood kraft pulp (LBKP), semi-bleached hardwood kraft pulp (LSBKP), unbleached hardwood sulfite pulp (LUSP), bleached hardwood sulfite pulp (LBSP), and semi-bleached hardwood sulfite pulp (LSBSP). In particular, a combination of bleached softwood kraft pulp (NBKP) and bleached hardwood kraft pulp (LBKP) is preferred.
[0019] Because softwood chemical pulp has a longer and thicker fiber structure than hardwood chemical pulp, incorporating a large amount of softwood chemical pulp results in a base paper with a high porosity, allowing for efficient incorporation of transparency-enhancing materials. Soaking This is possible. However, if softwood chemical pulp is added in excess, the paper base for translucent paper will deteriorate, and a uniform translucent region cannot be formed. On the other hand, hardwood chemical pulp has a fine and short fiber structure, which improves the paper base, but if the blending ratio is increased, the paper base will have a low porosity, and the penetration of the transparency material will be insufficient. To increase transparency, a large amount of transparency material is added. Soaking Doing so would impair its recyclability. Furthermore, because hardwood chemical pulp has a thin, short fiber structure, it is easily coated with resin contained in transparency materials, making it difficult to break down during recycling as waste paper.
[0020] The mixing ratio of softwood chemical pulp to hardwood chemical pulp is preferably 80:20 to 51:49. A more preferable ratio is 75:25 to 55:45, and an even more preferable ratio is 70:30 to 60:40. By specifying the ratio of softwood chemical pulp to hardwood chemical pulp, a translucent paper with a balanced combination of transparency and recyclability can be obtained.
[0021] The Canadian standard water content of the aforementioned coniferous chemical pulp is preferably 400 to 700 mL. More preferably, the Canadian standard water content is 420 to 650 mL CSF, and even more preferably 450 to 600 mL CSF. When the Canadian standard water content is above the lower limit of the above numerical range, the voids in the base paper for translucent paper can be maintained, thus allowing the transparent material to be contained. Soaking It offers excellent properties. When the Canadian standard filtration rate is below the upper limit of the aforementioned numerical range, the form of the base paper for translucent paper can be improved, making it easier to obtain translucent paper with a translucent region that is excellent in transparency and visibility.
[0022] The Canadian standard water content (CSF) of the hardwood chemical pulp is preferably 350 to 650 mL. More preferably 370 to 630 mL CSF, and even more preferably 400 to 600 mL CSF. If the Canadian standard water content is above the lower limit of the above numerical range, the strength of the base paper for translucent paper can be increased. If the Canadian standard water content is below the upper limit of the above numerical range, the form of the base paper for translucent paper can be improved, making it easier to obtain translucent paper with a translucent area that is excellent in transparency and visibility.
[0023] Furthermore, it is preferable for softwood chemical pulp to have a higher Canadian standard of filtration than hardwood chemical pulp, as this results in superior paper strength and transparency. The Canadian standard of filtration for pulp is measured according to JIS P8121-2:2012. Incidentally, glassine paper, which has been commonly known as a translucent paper, uses chemical pulp with a high degree of beating, for example, chemical pulp with a Canadian standard of filtration of 250 mlCSF or less. However, because the pulp fibers with a high degree of beating are ground and cut, they are difficult to apply to applications where strength is required, such as packaging bags, although they may be suitable for transparent windows on envelopes.
[0024] Other types of pulp besides softwood chemical pulp and hardwood chemical pulp can be used in combination with the pulp, as long as they do not impair the effects of the present invention. Examples include mechanical pulp, thermomechanical pulp, deinked pulp, non-wood pulp, and synthetic pulp.
[0025] The air permeability of the base paper for translucent paper is preferably 10 to 40 seconds. Preferably, it is 12 to 35 seconds, and more preferably 15 to 33 seconds. If the air permeability is above the lower limit of the above numerical range, the paper gains sufficient strength, resulting in translucent paper suitable for applications such as packaging paper and printing paper. If the air permeability is below the upper limit of the above numerical range, the permeability of the transparency material is excellent, and the transparency of the translucent paper can be enhanced. Air permeability is measured according to the Wang Research method of air permeability measured in accordance with J.TAPPI-5-2:2000.
[0026] The density of the base paper for translucent paper is 0.5 to 0.85 g / cm³. 3 Preferably, it is 0.6 to 0.8 g / cm³. 3 This is more preferable. If the density is above the lower limit of the above numerical range, the paper strength is obtained, resulting in a translucent paper suitable for applications such as packaging paper and printing paper. If the density is below the upper limit of the above numerical range, the permeability of the transparency material is excellent, and the transparency of the translucent paper can be increased. The density is measured in accordance with JIS P8118.
[0027] The porosity of the base paper for translucent paper is preferably 30-80%, more preferably 40-70%, and even more preferably 50-70%. If the porosity of the base paper for translucent paper is above the lower limit of the above numerical range, the transparency of the translucent region is easily enhanced. If the porosity of the base paper for translucent paper is below the upper limit of the above numerical range, the physical strength of the sheet is less likely to decrease. The porosity of the paper substrate is calculated from the value obtained by dividing the density measured according to JIS P8118 by the true density of cellulose, which is 1.50.
[0028] The ParkerPrintSurf smoothness of at least one side of the base paper for translucent paper is preferably 7 μm or less, and more preferably 5 μm or less. There is no particular lower limit. The smaller the value, the smoother the surface. ParkerPrintSurf smoothness can evaluate the smoothness of fine details, and the smaller this value, the less light scattering on the paper surface can be reduced, thus improving visibility through the translucent portion. ParkerPrintSurf smoothness is determined in accordance with ISO 8791-4:1992 (soft backing / clamp pressure 500 kPa).
[0029] In addition to pulp, the base paper for translucent paper may contain known papermaking aids such as paper strength enhancers, sizing agents, fillers, and colorants as appropriate. However, since the addition of fillers tends to increase the opacity of the paper, it is preferable to limit the amount to a level that does not impair transparency and visibility, and it is even preferable not to add fillers to the base paper for translucent paper.
[0030] The method for manufacturing base paper for translucent paper is not particularly limited. For example, a method may include a step of beating pulp which will be the raw material for the base paper for translucent paper, a step of papermaking a pulp slurry containing the beated pulp, and a step of drying the wet sheet obtained by papermaking.
[0031] In the beating process, it is preferable to beating the raw pulp so that it achieves the Canadian standard water content. The beating machine is not particularly limited. For example, known beating machines such as double disc refiners can be used. The papermaking machines used are not particularly limited. Examples include screenprint machines, short screenprint machines, and cylinder screenprint machines. The drying process is not particularly limited. For example, a dryer attached to the paper machine can be used.
[0032] The base paper for translucent paper may be subjected to a smoothing treatment. By applying a smoothing treatment, light scattering on the paper surface can be reduced, thereby improving visibility through the translucent portion. Examples of smoothing treatments include tightness pressing, machine calendering, gloss calendering, soft nip calendering, and supercalendering. However, these devices increase the density of the paper, so care must be taken to reduce the linear pressure to prevent the density from becoming too high. On the other hand, a transfer method in which the paper is attached to a smooth surface while it is still wet and then the smooth surface is transferred by drying is preferable because it does not increase the density of the paper. For example, technologies such as Yankee cylinders, cast drums, and film transfers can be used. Among these, a Yankee dryer using a Yankee cylinder is preferable because it is attached to the paper machine and offers excellent productivity.
[0033] (transparent material) The transparent material is included in the translucent paper base paper. Soaking By doing so, Soaking The material is not particularly limited as long as the part that is transparent becomes semi-transparent. For example, examples of transparency materials include resins such as acrylic resin, polyethylene resin, polyester resin, urethane resin, nitrocellulose, shellac, and rosin; vegetable oils such as tung oil, linseed oil, castor oil, hydrophilic castor oil, coconut oil, soybean oil, and commercially available salad oil; and waxes such as kaunaba wax, palm wax, beeswax, whale wax, and wood wax. One type of transparency material may be used alone, or two or more types may be used in combination.
[0034] Among these, resins that are stable over time are preferred, and acrylic resins are more preferred. Among acrylic resins, ultraviolet-curable acrylic resins are particularly preferred because they have excellent surface coverage and the interface of the region impregnated with the transparent material becomes clear in cross-sectional view. For example, an example of an ultraviolet-curable acrylic resin is the one disclosed in paragraphs 0025 and 0026 of Japanese Patent Application Publication No. 2021-91481.
[0035] As the transparency material, it is preferable to select one from the examples above that has a refractive index within the range of 1.4 to 1.6, preferably 1.45 to 1.58, more preferably 1.50 to 1.58, and even more preferably 1.52 to 1.58. This is because the refractive index of cellulose fibers is generally said to be within the range of 1.4 to 1.6. When the refractive index of the transparency material is within the above numerical range, the difference with the refractive index of the cellulose fibers is small, making it easier to improve the transparency and visibility of the semi-transparent region. The refractive index of the transparency material is measured according to JIS K 7142.
[0036] By impregnating a translucent base paper with a refractive index close to that of cellulose fibers and filling the voids between cellulose fibers within the paper, the refraction of light caused by the transparent material within the translucent base paper can be reduced. Therefore, a translucent region with excellent transparency and visibility can be easily obtained. High refractive index materials such as zirconium and titanium may be used as needed to adjust the refractive index.
[0037] Since the transparency material is applied to and impregnated into the base paper for semi-transparent paper, it is preferable that it be a liquid at room temperature or when heated. Furthermore, materials that can be dissolved in a liquid medium such as an organic solvent at room temperature or when heated are also preferable in terms of permeability. In other words, it is preferable that the transparency material be a permeable liquid transparency agent that can be impregnated into the base paper for semi-transparent paper during manufacturing.
[0038] To reduce the diffuse reflection of light caused by surface irregularities in the translucent region of the translucent paper, a coating layer may be provided on at least a portion of the surface of the translucent region. This coating layer increases the smoothness of the surface of the translucent region, prevents diffuse reflection of light on the surface of the translucent region, and improves the visibility of the translucent region. Examples of materials for the coating layer include transparency materials and OP varnish. Examples of transparency materials are the same as those exemplified in the section on translucent regions. When the coating layer contains a transparency material, the transparency material of the coating layer and the transparency material of the translucent region may be the same or of different types. Furthermore, one type of material may be used alone for the coating layer, or two or more types may be used in combination.
[0039] OP varnish is sometimes called overprint varnish. The composition of OP varnish varies depending on the product and manufacturer, but it is preferable to have OP varnish that contains at least one selected from the group consisting of linseed oil, tung oil, and nitrated cotton. Examples of commercially available OP varnishes include those from Toyo Ink Co., Ltd., T&K TOKA Corporation, and Fuji Ink Mfg. Co., Ltd. OP varnish may be used alone or in combination of two or more types. Drying methods may include oxidative polymerization or UV effect.
[0040] As the material for the coating layer, it is preferable to select one from among these that has a refractive index within the range of 1.4 to 1.6, preferably 1.45 to 1.60, more preferably 1.48 to 1.60, even more preferably 1.50 to 1.60, and particularly preferably 1.50 to 1.58. This is because the refractive index of cellulose fibers is generally said to be within the range of 1.4 to 1.6. By setting the refractive index of the coating layer to a value close to that of the cellulose fibers, the refraction of light at the interface between the coating layer and the base paper for translucent paper can be reduced. Therefore, it becomes easier to obtain a translucent region with excellent visibility. The refractive index of the coating layer is measured according to JIS K 7142.
[0041] When a coating layer is provided, the thickness of the coating layer is preferably 0.5 to 2.5 μm, more preferably 0.5 to 2.0 μm, and even more preferably 0.7 to 2.0 μm. If the thickness of the coating layer 5 is greater than or equal to the lower limit of the above numerical range, a glossy surface is obtained, and excellent visibility is easily obtained in the translucent region. If the thickness of the coating layer is less than or equal to the upper limit of the above numerical range, unevenness and curling of the paper sheet due to the difference in shrinkage after drying between the coated and uncoated parts is suppressed. The thickness of the coating layer is the value measured by taking a cross section perpendicular to the plane and observing the cross section with an electron microscope, and measuring the maximum value in the thickness direction.
[0042] The opacity of the translucent region is preferably 4-25%, more preferably 4-20%, and even more preferably 4-15%. The opacity of the translucent region is measured according to JIS P 8138:1976. A smaller opacity value indicates greater transparency.
[0043] A haze of 80% or less is preferable for the translucent region. A haze of 80% or less in the translucent region improves its transparency. The lower limit of the haze in the translucent region is not particularly limited, but for example, it is 10% or more, preferably 20% or more. The haze in the translucent region is measured according to JIS-K7136. A smaller haze value indicates less cloudiness.
[0044] Until now, haze and opacity have been used to evaluate the visibility of translucent areas. However, according to the inventors' research, the numerical trends of haze and opacity often do not correspond to the superiority or inferiority of visibility as perceived by the human eye. For example, when the whiteness of a sample is high, the transmittance of visible light is high, but this does not necessarily mean that the visibility or visual surface quality is superior.
[0045] The reason why the numerical trend of haze does not correspond to the superiority or inferiority of visibility is thought to be as follows: Haze is calculated as the ratio of diffuse transmittance to the total transmittance of light rays transmitted through a sample. Diffuse transmittance is the transmittance of diffuse light, obtained by excluding the parallel component of the light rays transmitted through a sample when linear light is incident on the sample. On the other hand, as shown in Figures 4 and 5, the human eye preferentially recognizes light that travels in a straight line or light with a narrow diffusion angle rather than diffuse light or scattered light with a wide diffusion angle. In calculating haze, parallel light components that are easily perceived by the human eye are excluded from the measurement target, while diffuse light that is difficult for the human eye to perceive is included in the measurement target to determine the diffuse transmittance. Since haze is calculated from this diffuse transmittance, it is not suitable for evaluating the perceived surface area by the human eye or the superiority or inferiority of visibility in the depth direction. Similarly, opacity is determined by including diffuse light, which is difficult for the human eye to perceive, in the measurement target, making it unsuitable for evaluating human visual perception of a surface or visibility in the depth direction.
[0046] As a result of diligent research, the inventors conceived the idea of evaluating the visibility of a translucent region based on the degree of blurring of the contents visible through the translucent region. The degree of blurring is due to the diffusion pattern of light transmitted through the translucent region. In the case of a translucent region with a high degree of blurring, a relatively large amount of diffused light with a wide diffusion angle is included in the transmitted light, thus reducing the visibility of the contents. Conversely, in the case of a translucent region with little blurring, a relatively large amount of light traveling in a straight line or light with a narrow diffusion angle is included in the transmitted light, resulting in good visibility of the contents. The inventors devised a method and index for quantitatively evaluating the degree of blurring, and found that if the index of blurring is above a certain value, the visibility of the contents viewed through the semi-transparent area is excellent. These indicators are luminous transmittance and luminous transmittance ratio.
[0047] "Measurement of luminous transmittance" For measuring luminous transmittance, a luminous transmittance meter is used that includes a light-emitting unit that projects light from a light source onto the sample, a light-receiving unit that receives the light transmitted through the sample, and a sensor that measures the received light. The distance between the light-emitting and light-receiving units must be 50 mm or more, and when measured without a sample, the light-receiving sensitivity characteristics should closely match those of the photopic standard relative luminous efficiency. Numerous luminous transmittance meters are commercially available for measuring eyeglass lenses, filter glass, transparent conductive film glass, etc., and measurements can be taken using any device that meets the above measurement conditions. In addition, any device that meets the above measurement conditions, such as a spectrophotometer, can be used as a luminous transmittance meter.
[0048] "Luminous transmittance (T50)" In this invention, it is preferable that the luminous transmittance (T50) under the following measurement conditions is 20% or more. "Measurement Condition 1" Using a luminous transmittance meter with a gap of at least 50 mm between the light-emitting and light-receiving sections, The translucent region of the aforementioned paper is used as a sample for measurement. The luminous transmittance measured when one side of the sample is placed in contact with the light source.
[0049] Figure 6 is an explanatory diagram illustrating the measurement. The luminous transmittance (T50) can be measured by placing one surface S1 of the sample S in contact with the light-emitting section 101 of the luminous transmittance meter 100. In this invention, the TLV-304-LC from Asahi Spectroscopic Co., Ltd., which is sold as a luminous transmittance meter, was used. In this device, the distance between the light-emitting section and the light-receiving section is 51.5 mm. By setting the luminous transmittance (T50) at a distance of at least 50 mm to 20% or more, the paper will have a transparent area with excellent visibility. The larger the value, the better the visibility, preferably 23% or more. Luminous transmittance (T50) is measured at a distance of 50 mm from the sample, rather than immediately after the light is emitted. This measurement excludes light that is scattered over that 50 mm and does not reach the light-receiving area, thus matching the perceived visibility. Since light does not scatter in air, the cause of scattering is due to the internal and surface conditions of the sample.
[0050] "Luminous transmittance ratio" In the present invention, it is preferable to have a translucent region in which the luminous transmittance ratio under the following measurement conditions is 44 or higher. "Measurement Condition 2" Using a luminous transmittance meter with a gap of at least 50 mm between the light-emitting and light-receiving sections, The translucent region of the aforementioned paper is used as a sample for measurement. The luminous transmittance (T50) measured when the sample is placed with one side in contact with the light source, The luminous transmittance (T0) is measured when the other side of the sample is placed in contact with the light-receiving part, and the luminous transmittance ratio is calculated using the following formula. Formula 1: Luminous transmittance ratio = (T50 / T0) × 100
[0051] Figures 7(a) and 7(b) are explanatory diagrams illustrating the measurement. The luminous transmittance (T50) can be measured by placing one surface S1 of the sample S in contact with the light-emitting section 101 of the luminous transmittance meter 100 (a). The luminous transmittance (T0) can be measured by placing the other surface S2 of the sample in contact with the light-receiving section 102 (b). When measuring the luminous transmittance (T0), it is advisable to hold the sample in place with a ring-shaped jig or similar to prevent it from bending due to its own weight. In this invention, the TLV-304-LC from Asahi Spectroscopic Co., Ltd., which is sold as a luminous transmittance meter, was used. In this device, the distance between the light-emitting section and the light-receiving section is 51.5 mm. The luminous transmittance ratio = (T50 / T0) × 100 is calculated from the luminous transmittance (T50) and luminous transmittance (T0) of two points at least 50 mm apart. By making this value 44 or higher, the paper will have a transparent area with excellent visibility. The higher the value, the better the visibility; preferably it is 48 or higher, and more preferably 50 or higher. The luminous transmittance ratio indicates how much the light transmitted from the sample decreased from (T0), measured immediately after it was emitted, to (T50), measured at a distance of 50 mm. (T50) excludes the light that was scattered over the 50 mm distance and did not reach the light-receiving part, thus corresponding to visibility. Since light does not scatter in air, the cause of scattering is due to the internal and surface conditions of the sample.
[0052] Furthermore, it is even more preferable to satisfy both the "luminous transmittance (T50)" and the "luminous transmittance ratio" mentioned above.
[0053] In order to achieve a luminous transmittance (T50) of 20% or more and a luminous transmittance ratio of 44 or more in the transparent region, it is advisable to control the refraction and scattering of light at the surface of the paper into which light is incident, the interior of the paper into which the incident light is felt, and the surface of the paper into which transmitted light is felt.
[0054] The density of the translucent region in translucent paper is 0.7 to 2.5 g / cm³. 3 Preferably, 0.7 to 2.0 g / cm³ 3 More preferably, 0.8-2.0 g / cm³ 3This is even more preferable. If the density of the translucent region is above the lower limit of the numerical range, it is considered that the air layer between the cellulose fibers has been sufficiently eliminated by impregnation with resin components. If the density of the translucent region is below the upper limit of the numerical range, the processability of the translucent paper when used as packaging material is improved. The density of the translucent region is measured in accordance with JIS P 8118.
[0055] The translucent paper of the present invention can be recycled without sorting. Generally, in paper recycling, collected waste paper is disintegrated in a large pulper called a pulper at a paper-pulp concentration of about 1%, undispersed material is removed in a coarse pulper of about 9 mm in diameter, and then further dispersed and fine undispersed material is removed by passing it through a cleaner or a screen of about 1.6 mm in diameter. If there is an excessive amount of resin, the disintegration and dispersibility deteriorates, which can clog these screens, or undispersed material can be brought into the paper as dust during the papermaking process, causing dust spots. For this reason, it is necessary to ensure that there are no undispersed materials such as fragments after redisintegration. The translucent paper of the present invention improves transparency by specifying the basis weight of the base paper, the amount of coating / impregnation of the transparency material, etc., and their ratio, thereby improving transparency with the transparency material and the content of the transparency material Soaking This allows for both the suppression of the resulting decline in recyclability and the mitigation of the problem.
[0056] (Manufacturing method for semi-transparent paper) The present invention relates to a method for producing translucent paper, which involves coating at least a portion of a base paper for translucent paper with a transparency material. Soaking Applying and / or containing the liquid Soaking A method for manufacturing translucent paper that forms a translucent region, characterized in that it satisfies all of the following requirements (1) to (3). Requirement (1): The basis weight (W) of the base paper for translucent paper is 30-100 g / m². 2 Requirement (2): Coating / containment per unit area of the translucent region Soaking Quantity (C) is 10-70g / m 2 Requirement (3): The value of C / (W+C)×100 is 20-40%
[0057] As mentioned above, for base paper for translucent paper, by satisfying requirements (1) to (3), the transparency is improved by the transparency material and the content of the transparency material Soaking This allows for both the suppression of the resulting decline in recyclability and the mitigation of the problem.
[0058] The application and impregnation of the transparency material involves applying a liquid transparency material to the base paper for semi-transparent paper. Soaking It penetrates by being applied or contained. Soaking The process can be performed on either side of the translucent paper base. If the ParkerPrintSurf smoothness of one side of the translucent paper base is 5 μm or less, the transparency material is applied to the other side. Soaking This is preferable because it allows for efficient penetration. If the Parker Printsurf smoothness is 5 μm or less on both sides, apply and incorporate it on the side with the higher value. Soaking It is recommended to do so. A surface with a low Parker Print Surf smoothness value has high smoothness, and therefore the density of cellulose fibers is higher closer to the surface. Therefore, applying and incorporating it into surfaces with low cellulose density is recommended. Soaking This allows the transparency material to penetrate. On the other hand, a Parker Printsurf smoothness of 5 μm or less is preferable because it is smooth, which suppresses light scattering on the paper surface, resulting in excellent visibility.
[0059] If the clearing material is solid at room temperature, a liquid medium capable of dissolving the clearing material is used for coating and impregnation. Soaking Prepare the solution. If the clearing material is liquid at room temperature, the concentration of the clearing material may be changed using a liquid medium, or it may be applied or incorporated directly without using a liquid medium. Soaking It may also be used as a liquid.
[0060] The liquid medium is not particularly limited. Either aqueous solvents or organic solvents can be used. If the liquid medium contains water, the base paper for translucent paper tends to swell due to the water. Furthermore, the base paper for translucent paper tends to shrink during subsequent drying. As a result, curling, bumping, and unevenness are likely to occur. Therefore, it is preferable that the liquid medium does not contain water, and organic solvents are more preferable.
[0061] The organic solvent may be a polar solvent or a nonpolar solvent. Examples of polar solvents include alcohols, ethers, esters, and nonpolar solvents. Examples of alcohols include methanol, ethanol, n-propanol, isopropanol, n-butanol, n-pentanol, and n-hexanol. Examples of ethers include ethylene glycol monomethyl ether, diethylene glycol monomethyl ether, triethylene glycol monomethyl ether, tetraethylene glycol monomethyl ether, ethylene glycol monoethyl ether, diethylene glycol monoethyl ether, triethylene glycol monoethyl ether, tetraethylene glycol monoethyl ether, ethylene glycol monopropyl ether, diethylene glycol monopropyl ether, triethylene glycol monopropyl ether, tetraethylene glycol monopropyl ether, ethylene glycol monoisopropyl ether, diethylene glycol monoisopropyl ether, triethylene glycol monoisopropyl ether, tetraethylene glycol monoisopropyl ether, ethylene glycol monobutyl ether, diethylene glycol monobutyl ether, triethylene glycol monobutyl ether, tetraethylene glycol monobutyl ether, ethylene glycol monoisobutyl ether, diethylene glycol monoisobutyl ether, triethylene glycol Polyethylene glycol monoisobutyl ether, tetraethylene glycol monoisobutyl ether, ethylene glycol monotertiary butyl ether, diethylene glycol monotertiary butyl ether, triethylene glycol monotertiary butyl ether, tetraethylene glycol monotertiary butyl ether, propylene glycol monomethyl ether, dipropylene glycol monomethyl ether, tripropylene glycol monomethyl ether, propylene glycol monoethyl ether, dipropylene glycol monoethyl ether, tripropylene glycol monoethyl ether, tetrapropylene glycol monoethyl ether, propylene glycol monopropyl ether, dipropylene glycol monopropyl ether, tripropylene glycol monopropyl ether, propylene glycol monoisopropyl ether, dipropylene glycol monoisopropyl ether, tripropylene glycol monoisopropyl ether, dipropylene glycol monobutyl ether, tripropylene glycol monobutyl ether, propylene glycol monoisobutyl ether,Examples of various glycol ethers include dipropylene glycol monoisobutyl ether, tripropylene glycol monoisobutyl ether, propylene glycol monotertiary butyl ether, dipropylene glycol monotertiary butyl ether, and tripropylene glycol monotertiary butyl ether. Examples of esters include diethylene glycol monoethyl ether acetate and diethylene glycol monobutyl ether acetate. Examples of nonpolar solvents include paraffinic hydrocarbons such as pentane, hexane, heptane, octane, nonane, decane, and dodecane; isoparaffinic hydrocarbons such as isohexane, isooctane, and isododecane; alkylnaphthenic hydrocarbons such as liquid paraffin; aromatic hydrocarbons such as benzene, toluene, xylene, alkylbenzene, and solvent naphtha; and silicone oil.
[0062] Coating / containing Soaking The liquid may further contain other components besides the clarifying material and liquid medium. Examples of other components include basic substances such as ammonia, ethylenediamine, and triethylamine; viscosity modifiers such as glycerin and ethylene glycol; high refractive index substances such as zirconium and titanium; defoaming agents; release agents; and colorants. However, other components are not limited to these examples.
[0063] Coating / containing Soaking In this case, the transparency material is applied to the cross-section of the base paper for translucent paper. Soaking A portion that does not reach the opposite side of the surface may be formed. In this portion, the surface condition of the surface with relatively high smoothness is achieved by applying a transparent material. Soaking This is because it allows the previous state to be maintained. Coating / containing Soaking In this case, the transparency material may be impregnated into both sides of the base paper for semi-transparent paper. Soaking This is in order to do so thoroughly. Tooru No brightening material included Soaking This is to reduce the amount of air gaps.
[0064] Coating / containing Soaking The application / impregnation rate of the liquid per unit area is 10-70 g / m². 2 Preferably, 20-60 g / m 2 More preferably, 30-60 g / m 2 This is even more preferable. Application / Containment Soaking Application and content of liquid per unit area Soaking When the amount is above the lower limit of the aforementioned numerical range, it is easier to increase the transparency of the translucent area. Soaking Application and content of liquid per unit area Soaking If the quantity is below the upper limit of the aforementioned numerical range, the recyclability can be improved.
[0065] Coating / containing Soaking The viscosity of the liquid is preferably 50 to 5000 mPa·s, more preferably 50 to 4000 mPa·s, and even more preferably 50 to 3000 mPa·s. If the viscosity is below the upper limit of the above numerical range, coating and inclusion Soaking The liquid penetrates easily into the paper, and the transparency of the translucent areas is enhanced. When the viscosity is above the lower limit of the aforementioned numerical range, the boundary between the translucent and non-translucent areas becomes clear. Viscosity is measured using a Blookfield viscometer under conditions of 30°C and 60 rpm.
[0066] Coating / containing Soaking The method of applying the liquid is not particularly limited. Examples include flexographic printing, inkjet printing, gravure printing, offset printing, gravure offset printing, screen printing, roll coating, bar coating, and blade coating. Among these, using a printing method is preferable because it makes it easy to align the semi-transparent portion, and in the case of a multi-color printing press, the application and inclusion of the liquid are possible. Soaking Apply the liquid in multiple layers. Soaking It is preferable because it allows for this.
[0067] Coating containing a transparency material Soaking By impregnating the base paper for translucent paper with a liquid, the voids between the cellulose fibers in the translucent paper can be filled with a transparency material. The coating / implantation includes a transparency material with a refractive index in the range of 1.4 to 1.6. SoakingWhen using a liquid, the voids within the translucent paper can be filled with a transparency material that has a refractive index close to that of cellulose. Therefore, the refraction of light caused by the voids within the translucent paper can be reduced.
[0068] Coating / containing Soaking Inclusion of the liquid into the base paper for translucent paper Soaking The coating may be performed in a single step or in multiple steps. If performed in multiple steps, the components and composition of the transparency material used in each step may be the same or different.
[0069] When using an ultraviolet-curing clearing agent, various light sources can be used, such as high-pressure mercury lamps, metal halide lamps, xenon lamps, and electrodeless discharge lamps. The cumulative light intensity is not particularly limited and can be appropriately adjusted depending on the amount of clearing agent used and the type of clearing resin.
[0070] (semi-transparent area) The translucent region is formed in a portion of the translucent paper when viewed from above. When the translucent paper is used as packaging, the contents and address can be seen from the outside of the packaging through the translucent region. The shape and area ratio of the translucent region in a planar view are not limited in any way. They can be set or changed as appropriate depending on the application of the packaging paper, packaging material, or printing paper. In other examples, the translucent region may be the entire area in the planar direction of the translucent paper. Furthermore, the number of translucent regions is not particularly limited and may be one or more. In the case of translucent paper with multiple translucent regions, the size and shape of each translucent region are not particularly limited.
[0071] (Application) The translucent paper of the present invention provides unprecedented transparency and visibility, as well as excellent recyclability. Therefore, it can be used not only as packaging paper, but also as printing paper, book paper, copy paper, information paper, label paper, etc., for various applications where an image (characters, symbols, pictures, objects, etc.) on the opposite side of the paper can be seen through the paper substrate. [Examples]
[0072] The present invention will be specifically described below with reference to examples, but the present invention is not limited to the following description.
[0073] (Preparation of chemical pulp) NBKP: Bleached softwood kraft pulp that has been beaten and filtered to a Canadian standard water content of 550 mL. LBKP: Hardwood bleached kraft pulp that has been beaten and filtered to a Canadian standard water content of 500 mL.
[0074] (Manufacturing of base paper for translucent paper) Using the chemical pulp formulations shown in Table 1, base paper for translucent paper was manufactured using a wireframe paper machine equipped with a Yankee dryer.
[0075] [Table 1]
[0076] (including Soaking Preparation of coating solution) Contains Soaking Coating solution 1: As a transparency material, an acrylic paraffin solvent (product name: Clariten DC, manufactured by Yamato Chemical Industry Co., Ltd.) was prepared. The refractive index of this transparency material is 1.50. The refractive index was measured using an Appe refractive index meter manufactured by Atago Co., Ltd. As a solvent, an aromatic paraffinic solvent (product name: Clariten S, manufactured by Yamato Chemical Industry Co., Ltd.) was prepared. These clearing materials and the solvent were mixed, and the concentration of the clearing material was 75% by mass. Soaking A coating solution was prepared. Soaking The viscosity of the coating solution at 30°C and 60 rpm was 1800 mPa·s. Contains SoakingA 2:40% shellac coating solution (manufactured by Koyo Chemical Co., Ltd.) was diluted with anhydrous ethanol from Ken-ei Pharmaceutical Co., Ltd. to prepare an alcohol-diluted shellac solution with a solid content of 25.0% by mass. The refractive index was 1.46. The refractive index was measured using an Appe refractive index meter manufactured by Atago Co., Ltd. Sumifix HF Navy2G gran solution (blue) manufactured by Sumika Chemtex Co., Ltd. was added dropwise to a concentration of 0.2% by mass relative to the total mass of this diluted solution, and dispersed using a rotation / revolution mixer, Awatori Rentaro ARE310, manufactured by Thinky Co., Ltd. Soaking A coating solution was prepared. Soaking The viscosity of the coating solution at 30°C and 60 rpm was 1200 mPa·s.
[0077] Examples 1-6, Comparative Examples 1-5 (Manufacturing of translucent paper) Using a Matsuo Sangyo micrometer adjustable applicator, the opposite side of the highly smooth surface of the translucent paper base obtained in Manufacturing Examples 1 to 8 was subjected to the following process: Soaking Coating solution 1 was applied and printed, and dried at 100°C for 5 minutes using a hot air circulation dryer from Heattech Co., Ltd. Soaking The quantities were set as shown in Tables 2 and 3.
[0078] Example 7 Furthermore, on the opposite side of the highly smooth surface of the translucent paper base obtained in Manufacturing Example 1, the above-mentioned Soaking The coating liquid 2 was impregnated and coated. Specifically, the rubber roll transfer method was used. Soaking The coating solution 2 was repeatedly applied and dried at room temperature to obtain a translucent paper. Soaking The quantities were adjusted as shown in Table 3.
[0079] (evaluation) The translucent papers obtained in Examples 1 to 7 and Comparative Examples 1 to 5, as well as commercially available glassine paper as Reference Example 1, were prepared.
[0080] [Opacity] The opacity was measured using the "SC-WT" (a product of Suga Test Instruments Co., Ltd.) which conforms to JIS P8149. "Luminous transmittance (T50)" The luminous transmittance (T50) was measured using the TLV-304-LC from Asahi Spectroscopic Co., Ltd. as the luminous transmittance meter, as shown in Figure 6.
[0081] "Luminous transmittance ratio" Using the TLV-304-LC from Asahi Spectroscopic Co., Ltd. as a luminous transmittance meter, the luminous transmittance (T50) and luminous transmittance (T0) were measured as shown in Figure 7, and the luminous transmittance ratio was calculated using the following formula. Formula 1: Luminous transmittance ratio = (T50 / T0) × 100
[0082] [Evaluation of visibility in the depth direction] A printed A4-sized Word document with 10.5-point font size was placed on a horizontal surface, and each example of packaging paper was positioned 5.0 cm above it. Furthermore, the visibility of the printed text was evaluated based on the following criteria when viewed from 50 cm above the packaging paper, through the translucent area of the packaging paper. A: The letters are all clearly recognizable with no missing characters. B: There are slight missing letters, but the letters are clearly recognizable. C: Some characters are missing, but the characters are recognizable. C': The lighting is a bit dim, but the text is recognizable. D: Multiple characters are missing, making the text difficult to read. E: Characters are missing in many places, making them extremely difficult to recognize as letters.
[0083] "Recyclability" As part of the assessment of recyclability, the following redissociation assessment was performed. The resulting translucent paper was torn by hand into 10mm squares, and 500ml of the mixture, with a concentration of 3%, was stirred for 30 seconds in a household mixer, a Tescom TM856-W mixer, and then sieved through a HOGA 12-mesh sieve. ◎: Successfully filtered ○: The weight of the dried material was 0.5g or less, even though it could not be sieved. ×: Although it could not be sieved, its weight after drying exceeded 0.5g.
[0084] [Table 2]
[0085] [Table 3]
[0086] The translucent paper used in the example exhibited excellent transparency and visibility, as well as good decomposition properties. [Industrial applicability]
[0087] According to the present invention, a translucent paper is provided that offers excellent visibility when viewed through a translucent area and is suitable for recycling even after being collected as waste paper. [Explanation of symbols]
[0088] 1 (1A, 1B)...Translucent paper, 2...Base paper for translucent paper, 3...Transparency material, 4...Translucent region, 5...Coating layer, 10...Packaging, 11...Target image, 12...Visible image, F...Resin film, 100...Luminous transmittance meter, 101...Light emitting unit, 102...Light receiving unit, S...Sample, S1...One side of the sample, S2...Other side of the sample.
Claims
1. A base paper for translucent paper, and a translucent paper having a translucent region formed by coating or impregnating at least a portion of the base paper with a transparency material, The aforementioned base paper for translucent paper mainly consists of coniferous chemical pulp and hardwood chemical pulp. The ratio of the aforementioned coniferous chemical pulp to the aforementioned hardwood chemical pulp is 80:20 to 51:
49. The Canadian standard filtration rate of the aforementioned coniferous chemical pulp is 400 to 700 mL. The refractive index of the transparent material is 1.4 to 1.
6. A translucent paper characterized by satisfying all of the following requirements (1) to (3). Requirement (1): The basis weight (W) of the base paper for translucent paper must be between 30 and 100 g / m². 2 Requirement (2): The coating / impregnation amount (C) per unit area of the translucent region is 10 to 70 g / m². 2 Requirement (3): The value of C / (W+C)×100 is between 20% and 40%.
2. The translucent paper according to claim 1, wherein the transparent material is at least one or more selected from the group consisting of acrylic resin, polyethylene resin, polyester resin, urethane resin, nitrocellulose, shellac, rosin, tung oil, linseed oil, castor oil, hydrophilic castor oil, coconut oil, soybean oil, salad oil, kaunaba wax, palm wax, beeswax, whale wax, and wood wax.
3. The translucent paper according to claim 1, wherein the base paper for translucent paper contains coniferous chemical pulp and hardwood chemical pulp, and the ratio of the coniferous chemical pulp to the hardwood chemical pulp is 75:25 to 55:
45.
4. The translucent paper according to claim 1, wherein the refractive index of the transparent material is 1.45 to 1.
6.
5. The translucent paper according to claim 1, wherein the translucent region has a luminous transmittance (T50) of 20% or more under the measurement condition 1 described below. "Measurement Condition 1" Using a luminous transmittance measuring instrument with a gap of at least 50 mm between the light-emitting and light-receiving parts, The sample used to measure the translucent region of the aforementioned translucent paper is: The luminous transmittance (T50) measured when the sample is placed with one side in contact with the light source.
6. The translucent paper according to claim 1 or 5, wherein the translucent region has a luminous transmittance ratio of 44 or more under the measurement condition 2 described below. "Measurement Condition 2" Using a luminous transmittance measuring instrument with a gap of at least 50 mm between the light-emitting and light-receiving parts, The translucent region of the aforementioned paper is used as a sample for measurement. The luminous transmittance (T50) measured when the sample is placed so that one side is in contact with the light source, The luminous transmittance (T0) is measured when the other side of the sample is placed in contact with the light-receiving part, and the luminous transmittance ratio is calculated using the following formula. Formula 1: Luminous transmittance ratio = (T50 / T0) × 100
7. A method for producing translucent paper, comprising applying and / or impregnating a coating / impregnation solution containing a transparency material to at least a portion of a base paper for translucent paper to form a translucent region, The aforementioned base paper for translucent paper mainly consists of coniferous chemical pulp and hardwood chemical pulp. The ratio of the aforementioned coniferous chemical pulp to the aforementioned hardwood chemical pulp is 80:20 to 51:
49. The Canadian standard filtration rate of the aforementioned coniferous chemical pulp is 400 to 700 mL. The refractive index of the transparent material is 1.4 to 1.
6. A method for manufacturing translucent paper, characterized by satisfying all of the following requirements (1) to (3). Requirement (1): The basis weight (W) of the base paper for translucent paper must be between 30 and 100 g / m². 2 Requirement (2): The coating / impregnation amount (C) per unit area of the translucent region is 10 to 70 g / m². 2 Requirement (3): The value of C / (W+C)×100 is between 20% and 40%.
8. The method for producing translucent paper according to claim 7, wherein the transparent material is at least one or more selected from the group consisting of acrylic resin, polyethylene resin, polyester resin, urethane resin, nitrocellulose, shellac, rosin, tung oil, linseed oil, castor oil, hydrophilic castor oil, coconut oil, soybean oil, salad oil, kaunaba wax, palm wax, beeswax, whale wax, and wood wax.
9. A method for producing translucent paper according to claim 7, wherein the base paper for translucent paper contains coniferous chemical pulp and hardwood chemical pulp, and the ratio of the coniferous chemical pulp to the hardwood chemical pulp is 75:25 to 55:
45.
10. The Canadian standard filtration rate of the aforementioned coniferous chemical pulp is 400 to 700 mL. The Canadian standard filtration capacity of the aforementioned hardwood chemical pulp is 350 to 650 mL. A method for producing translucent paper according to claim 9.
Citation Information
Patent Citations
Roduction of transparent paper
JP1986132698A
Production of transparent paper
JP1986132699A
Paper excellent in barrier property, transparency and further dimensional stability and its production
JP1993247896A
Paper for envelope with window, and method for producing paper for envelope with window
JP2007262599A
Fiber composite material and method for producing the same
JP2008024778A