Resin particles, toner, developer, and toner storage unit
Resin particles with a core-shell structure and specific plant-derived alcohol monomer distribution address heat resistance and storage issues in toners, enhancing environmental sustainability and performance.
Patent Information
- Application Number
- JP2022191445
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-11-30
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2042-11-30
AI Technical Summary
Existing toners using plant-derived resins face issues with reduced heat resistance, storage properties, and strength, leading to problems such as filming, and existing solutions do not adequately address environmental impact and manufacturing energy consumption.
Resin particles with a core-shell structure, where the first resin contains 5-30% plant-derived alcohol monomer units and the second resin contains 2-30% plant-derived alcohol monomer units, with a specific distribution of non-plant-derived resin on the surface to enhance heat resistance and storage properties without using newly synthesized materials.
The solution provides toners with excellent heat resistance and storage properties while reducing environmental impact and manufacturing energy, maintaining strength by controlling resin composition and position.
Smart Images

Figure 0007947945000001 
Figure 0007947945000002
Abstract
Description
[Technical Field]
[0001] The present invention relates to resin particles, toner, developer, and toner storage unit. [Background technology]
[0002] In recent years, there has been a growing demand for toners to reduce their environmental impact. To this end, measures such as reducing energy consumption during manufacturing and adopting plant-derived resins for binders are being considered. However, it is known that using plant-derived resins can reduce the strength of the toner, impair its heat resistance and storage properties, and lead to problems such as filming issues.
[0003] Patent Document 1 discloses a technology that includes polyethylene terephthalate in the binder resin of the core and shell. Patent document 2 proposes using plant-derived resins in polymerized toners that require less manufacturing energy. [Overview of the project] [Problems that the invention aims to solve]
[0004] However, Patent Document 1 does not mention the inclusion of plant-derived alcohol monomers in the alcohol component of the core binder resin, and therefore, it cannot be said that the reduction in environmental impact is sufficient. Furthermore, even when using plant-derived resins in toner, as described in Patent Document 2, the heat resistance and storage properties are poor, and the strength of the toner decreases when plant-derived resins are used, leading to problems such as filming, making it difficult to achieve satisfactory quality.
[0005] The present invention aims to provide a toner that uses plant-derived resins, requires less newly synthesized materials, reduces manufacturing energy and environmental impact, and has excellent heat resistance and storage properties. [Means for solving the problem]
[0006] To solve the above problems, the present invention provides Resin particles having a core-shell structure comprising a first resin and a second resin, The first resin contains, in 100 mol% of alcohol monomer units, 5 mol% to 30 mol% of plant-derived alcohol monomer units. The second resin contains, in 100 mol% of alcohol monomer units, 2 mol% to 30 mol% of plant-derived alcohol monomer units. The present invention provides resin particles characterized in that, in the outermost resin when the shell layer in the core-shell structure is divided into 10 equal parts in the diametrical direction, the signal peak intensity of monomer units of non-plant-derived resins other than PET and PBT is 5 times or more than the sum of the signal peak intensity of plant-derived alcohol monomer units obtained by nano IR measurement and the signal peak intensity of monomer units derived from at least one of PET and PBT. [Effects of the Invention]
[0007] This invention allows for the use of plant-derived resins, reduces the amount of newly synthesized materials used, lowers manufacturing energy and environmental impact, and provides a toner with excellent heat resistance and storage properties. [Modes for carrying out the invention]
[0008] Normally, when resins made from plant-derived alcohol monomers are used in toners, the strength of the resin particles decreases and they aggregate at high temperatures. Therefore, it is necessary to increase the toughness of the resin particles by using resins containing BPA-PO (bisphenol A-propylene oxide adduct) or BPA-EO (bisphenol A-ethylene oxide adduct) on the surface of the resin particles. However, using newly chemically synthesized BPA-PO or BPA-EO as alcohol components presents a problem in terms of increased environmental impact.
[0009] As a result of intensive studies, the present inventors have found that, although the use of a resin containing a plant-derived alcohol monomer unit has a problem of reduced heat-resistant storage stability, the use of the resin particles of the present invention can provide a toner excellent in heat-resistant storage stability while reducing environmental load by using the resin containing a plant-derived alcohol monomer unit.
[0010] That is, the present invention relates to resin particles having a core-shell structure including a first resin and a second resin, wherein the first resin contains 5 mol% or more and 30 mol% or less of a plant-derived alcohol monomer unit in 100 mol% of all alcohol monomer units, the second resin contains 2 mol% or more and 30 mol% or less of a plant-derived alcohol monomer unit in 100 mol% of all alcohol monomer units, in the outermost resin when the shell layer in the core-shell structure is equally divided into 10 parts in the diameter direction, the signal peak intensity of the non-plant-derived resin monomer unit excluding PET and PBT, relative to the sum of the signal peak intensity of the plant-derived alcohol monomer unit obtained by nano-IR measurement and the signal peak intensity of the monomer unit derived from at least one of PET and PBT, is 5 times or more .
[0011] With the resin particles of the present invention, it is possible to control the abundance and position of each resin such that a large amount of the resin containing the non-plant-derived resin monomer unit is present only on the surface of the resin particles, and the resin containing the plant-derived alcohol monomer unit or the monomer unit derived from PET and / or PBT is mainly present inside the resin particles. Therefore, in the resin particles used for toner, it is possible to suppress a decrease in durability due to a decrease in heat-resistant storage stability or strength of the resin particles even without reducing the amount of non-plant-derived resin such as BPA-PO or BPA-EO, or without using BPA-PO or BPA-EO.
[0012] Hereinafter, embodiments of the present invention will be described in detail.
[0013] (Resin Particles) The resin particles according to the present embodiment are resin particles having a core-shell structure comprising a first resin and a second resin.
[0014] <Core-Shell Structure> The resin particles have a core-shell structure. As used herein, the term "core-shell structure" means a structure having a "core" composed of a core layer and a "shell" composed of a shell layer. The "shell layer" means a layer composed of a resin present in the outermost layer of the resin particles. The "core layer" means the region within the resin particles excluding the shell layer. The shell layer may contain part or all of the constituent elements of the core layer, and may have part or all of the core layer as domains or domain particles. The core layer and the shell layer are formed inhomogeneously without being completely compatible with each other. In the core-shell structure, it is preferable that the surface of the core layer is in a form coated with the shell layer. In the core-shell structure, the surface of the core layer may be completely coated with the shell layer, or may not be completely coated with the shell layer. Examples of the form in which the surface of the core layer is not completely coated with the shell layer include a form in which the core layer is coated with the shell layer in a mesh pattern, and a form in which the core layer is partially exposed from the shell layer. Among these, from the viewpoint of filming resistance, it is preferable that the surface of the core layer is completely coated with the shell layer.
[0015] <<Core>> The core can constitute the core portion in the resin particles having a core-shell structure. The core can contain the first resin. The first resin that can be contained in the core is an example of the resin in the present embodiment.
[0016] -First Resin- The first resin contains 5 mol% to 30 mol% of plant-derived alcohol monomer units per 100 mol% of alcohol monomer units.
[0017] In this specification, "plant-derived" refers to materials obtained from plant-derived raw materials (also called "biomass"). A monomer unit refers to the smallest unit that constitutes a polymer.
[0018] -Plant-derived monomer units- Plant-derived monomer units include plant-derived alcohol monomer units. Plant-derived acid units are not particularly limited as long as they are plant-derived; they can be appropriately selected according to the purpose. Examples include monomer units using acid monomers that can be substituted for plant-derived monomer units in resins. These may be used individually or in combination of two or more types. The resin having the aforementioned plant-derived monomer units has high carbon neutrality because it is plant-derived.
[0019] Here, "carbon neutrality" is generally used as a definition for plant-derived components that are composed of organic matter. When such plant-derived components are burned, carbon dioxide is emitted, but the carbon contained in this carbon dioxide originates from the carbon dioxide that the plant-derived component absorbed from the atmosphere through photosynthesis during its growth process. Therefore, even when plant-derived components are used, it is considered that the overall amount of carbon dioxide in the atmosphere does not increase. This property is called "carbon neutrality." A "highly carbon-neutral resin" refers to a resin that uses fewer newly synthesized materials, resulting in lower manufacturing energy consumption and environmental impact. Therefore, resins containing the aforementioned plant-derived monomer units can be said to have high carbon neutrality.
[0020] Furthermore, materials that were previously derived from petroleum, which are not plant-derived materials, can now be replaced with plant-derived materials. Ethylene glycol, propylene glycol, 1,3-propanediol, 1,4-butanediol, glycerin, succinic acid, itaconic acid, sebacic acid, and terephthalic acid are already being commercialized as plant-derived materials.
[0021] In this specification, there are no particular limitations on the monomer raw materials that can be used as monomer units to replace the plant-derived components, and they can be appropriately selected depending on the purpose. Examples include plant-derived ethylene glycol, plant-derived propylene glycol, plant-derived 1,3-propanediol, plant-derived 1,4-butanediol, plant-derived glycerin, plant-derived succinic acid, plant-derived itaconic acid, plant-derived sebacic acid, or plant-derived terephthalic acid. These may be used individually or in combination of two or more. The monomers that can be substituted for the aforementioned plant-derived components are preferably commercially available plant-derived monomers, as they are readily available; however, they may also be obtained by isolating them from plants as appropriate.
[0022] The content of plant-derived alcohol monomer units in the first resin is 5 mol% to 30 mol%, preferably 5 mol% to 20 mol%, relative to 100 mol% of the alcohol monomer units in the core resin.
[0023] If the amount of plant-derived alcohol monomer units in the first resin is less than 5 mol% of 100 mol%, the effect of reducing environmental impact will be small, and if it is more than 30 mol%, the shelf life will deteriorate.
[0024] -Measurement of plant-derived monomer units- 14 C concentration is present in nature (atmosphere), and while plants are active, it is taken into the plant through photosynthesis, and is part of the carbon dioxide present in the atmosphere. 14 C concentration and the carbon content in plant organic components14 C concentration is at an equilibrium (107.5 pMC). However, from the stage where plants cease their life activities, carbon uptake via photosynthesis stops, 14 Following the 5,730-year half-life of C, the 14 C concentration decreases. Since fossil resources derived from organisms have elapsed tens of thousands to hundreds of millions of years after the cessation of life activities, the aforementioned 14 C is hardly detected.
[0025] The aforementioned 14 C concentration can also define how much of the carbon in the carbon element components of carbon-containing petrochemical products is plant-derived carbon. Note that the concentration of 14 C in the carbon element of petrochemical products can be measured, for example, in accordance with ASTM-D6866, an ASTM standard of the American Society for Testing and Materials.
[0026] Here, "pMC" is an abbreviation for percent Modern Carbon, and is one of the units representing 14 C concentration. The ratio of 14 C to 12 C in biomass in the year 1950 A.D. ( 14 C / 12 C) is defined as 100 pMC.
[0027] 1 g of the resin particles or toner is placed into 100 mL of chloroform, and the mixture is stirred at 25°C for 30 minutes to obtain a solution in which the soluble content is dissolved. This is filtered through a membrane filter with an opening of 0.2 μm to obtain the chloroform-soluble content in the resin particles or toner. The chloroform-soluble content is dried at 45°C for 24 hours, then combusted, and the resulting CO₂ (carbon dioxide) is reduced to obtain C (graphite). The radiocarbon isotope 14 C concentration (hereinafter sometimes referred to as " 14 C concentration") is measured using an accelerator mass spectrometer (AMS: Accelerator Mass Spectroscopy, manufactured by Beta Analytic Inc.). Measured 14 By substituting the C concentration into the following formula (1), the "percentage of plant-derived components in resin particles or toner" can be calculated. Percentage of plant-derived components in resin particles (%) = 14 C concentration (pMC) / 107.5×100...Equation (1) Furthermore, measurement using AMS is disclosed, for example, in Japanese Patent No. 4050051.
[0028] -Amorphous polyester resin- The first resin preferably contains an amorphous polyester resin which is advantageous for low-temperature fixing, the amorphous polyester resin is more preferably a linear polyester resin, and even more preferably an unmodified polyester resin.
[0029] The amorphous polyester resin, which is a linear polyester resin, is preferably a polyester resin consisting of a linear main chain or a polyester resin having a structure consisting of a linear main chain and relatively short side chains bonded thereto.
[0030] The aforementioned amorphous polyester resin, which is an unmodified polyester resin, is preferably a polyester resin obtained using a polyhydric alcohol and a polyhydric carboxylic acid or its derivative, such as a polyhydric carboxylic acid, polyhydric carboxylic acid anhydride, or polyhydric carboxylic acid ester. Furthermore, it is preferable that this unmodified polyester resin is a polyester resin that has not been modified with isocyanate compounds or the like.
[0031] The amorphous polyester resin preferably does not have urethane bonds and urea bonds.
[0032] The amorphous polyester resin preferably contains a dicarboxylic acid component, and more preferably the dicarboxylic acid component contains 50 mol% or more of terephthalic acid. This is advantageous in terms of heat resistance and storage properties.
[0033] Examples of the aforementioned polyhydric alcohols include diols.
[0034] Examples of the aforementioned diols include alkylene (2-3 carbon atoms) oxide (average number of added moles 1-10) adducts of bisphenol A such as polyoxypropylene(2,2)-2,2-bis(4-hydroxyphenyl)propane and polyoxyethylene(2,2)-2,2-bis(4-hydroxyphenyl)propane; ethylene glycol; propylene glycol; hydrogenated bisphenol A; and alkylene (2-3 carbon atoms) oxide (average number of added moles 1-10) adducts of hydrogenated bisphenol A. These may be used individually or in combination of two or more.
[0035] Examples of the polycarboxylic acid include dicarboxylic acids.
[0036] Examples of dicarboxylic acids include succinic acids substituted with C1-C20 alkyl groups or C2-C20 alkenyl groups, such as adipic acid, phthalic acid, isophthalic acid, terephthalic acid, fumaric acid, maleic acid, dodecenyl succinic acid, and octyl succinic acid. These may be used individually or in combination of two or more. Among these, it is preferable to include saturated aliphatic succinic acid derived from plants.
[0037] Because the dicarboxylic acid is a plant-derived component, the carbon neutrality of the resin particles can be enhanced, thereby reducing the environmental impact. Furthermore, saturated aliphatic compounds have the effect of enhancing the recrystallization properties of crystalline polyester resins, thereby increasing the aspect ratio of the crystalline polyester resin and improving its low-temperature fixability. These can be used individually or in combination of two or more.
[0038] Furthermore, for the purpose of adjusting the acid value and hydroxyl value, amorphous polyester resin may contain at least one of a trivalent or higher carboxylic acid and a trivalent or higher alcohol at the end of its resin chain.
[0039] Examples of the carboxylic acids with a valency of 3 or higher include trimellitic acid, pyromellitic acid, or their acid anhydrides.
[0040] Examples of trivalent or higher alcohols include glycerin, pentaerythritol, and trimethylolpropane.
[0041] The molecular weight of the amorphous polyester resin is not particularly limited and can be appropriately selected depending on the purpose. For example, the molecular weight of the amorphous polyester resin is preferably 3,000 to 10,000 in GPC (Gel permeation chromatography) measurements, and more preferably 4,000 to 7,000. Furthermore, the number-average molecular weight (Mn) of the amorphous polyester resin is preferably 1,000 to 4,000, and more preferably 1,500 to 3,000. In addition, the Mw / Mn ratio is preferably 1.0 to 4.0, and more preferably 1.0 to 3.5.
[0042] When the molecular weight of the amorphous polyester resin is above the lower limit, it is possible to suppress a decrease in the heat resistance and durability of the toner against stress such as agitation in the developing machine when the resin particles are used in the toner. When the molecular weight of the amorphous polyester resin is below the upper limit, it is possible to suppress an increase in the viscoelasticity of the toner when it melts and suppress a decrease in low-temperature fixability.
[0043] There are no particular restrictions on the acid value of the amorphous polyester resin, and it can be appropriately selected depending on the purpose. The acid value of the amorphous polyester resin is preferably 1 mg KOH / g or more and 50 mg KOH / g or less, and more preferably 5 mg KOH / g or more and 30 mg KOH / g or less.
[0044] When the acid value of the amorphous polyester resin is 1 mg KOH / g or higher, the toner tends to become negatively charged when the resin particles are used in the toner. Furthermore, the affinity between the paper and the toner improves during fixing to paper, thereby improving low-temperature fixing performance. When the acid value is 50 mg KOH / g or lower, the decrease in electrostatic stability, particularly electrostatic stability against environmental fluctuations, can be suppressed.
[0045] There are no particular restrictions on the hydroxyl value of the amorphous polyester resin, and it can be appropriately selected depending on the purpose, but it is preferable that it is 5 mg KOH / g or higher. If the hydroxyl value of the amorphous polyester resin is 5 mg KOH / g or higher, the desired low-temperature fixability can be obtained.
[0046] The glass transition temperature (Tg) of the amorphous polyester resin is preferably 40°C to 80°C, and more preferably 50°C to 70°C.
[0047] If the glass transition temperature of the amorphous polyester resin is 40°C or higher, the toner will have sufficient heat resistance and durability against stress such as agitation in the developing machine when resin particles are used in the toner, and will also have good filming resistance. If the glass transition temperature is 80°C or lower, the deformation due to heating and pressurization during toner fixing when resin particles are used in the toner will be sufficient, resulting in good low-temperature fixing performance.
[0048] The molecular structure of the amorphous polyester resin can be confirmed by NMR (Nuclear Magnetic Resonance) measurements in solution or solid state, as well as by X-ray diffraction (XRD), GC / MS (Gas Chromatography - Mass Spectrometry), LC / MS (Liquid Chromatograph - Mass Spectrometry), and IR (Infrared Spectroscopy) measurements.
[0049] A simple method for detecting the amorphous polyester resin is to use an infrared absorption spectrum of 965±10 cm². -1 and 990±10cm -1 One method for detecting amorphous polyester resins is one in which those that do not exhibit absorption based on δCH (out-of-plane angular bending vibration) of olefins are identified.
[0050] There are no particular restrictions on the content of the amorphous polyester resin, and it can be appropriately selected depending on the purpose, but it is preferably 50% to 90% by mass, and more preferably 60% to 80% by mass, relative to 100% by mass of the first resin.
[0051] In the first resin, if the content of the amorphous polyester resin is 50% by mass or more, it is possible to suppress deterioration of the dispersibility of pigments and release agents in the toner when resin particles are used in the toner, and to suppress the occurrence of image blurring and distortion. If the content is 90% by mass or less, it is possible to suppress a decrease in low-temperature fixing performance, which is advantageous in that it is excellent in both high image quality and low-temperature fixing performance.
[0052] -Monomer units derived from PET and / or PBT- The first resin of the core may further contain monomer units derived from polyethylene terephthalate (hereinafter referred to as PET) and / or polybutylene terephthalate (hereinafter referred to as PBT). Both PET and PBT are crystalline thermoplastic saturated polyesters.
[0053] In this specification, "PET and / or PBT" indicates that the first resin may contain both PET and PBT, or either PET or PBT.
[0054] The aforementioned PET is generally composed of ethylene glycol and terephthalic acid. Furthermore, the aforementioned PBT is generally composed of butylene glycol and terephthalic acid. Therefore, examples of monomer units derived from PET and / or PBT include monomer units of ethylene glycol, butylene glycol, or terephthalic acid. In the first resin, the PET and / or PBT-derived components may or may not be included, but their inclusion is preferable in terms of heat resistance and filming resistance.
[0055] Both PET and PBT are semi-aromatic polyesters formed by the reaction of aromatic diacids with aliphatic diols. Specifically, the PET is a compound having an aromatic ring skeleton and a carbon number of C2 derived from the aliphatic diol. The PBT is a compound having an aromatic ring skeleton and a carbon number of C4 derived from the aliphatic diol.
[0056] Thus, because PET and PBT have similar chemical properties, it is common knowledge in this art that what can be done with PET can generally also be done with PBT. In the resin particles of the present invention, PET and PBT are interchangeable, and in the resin particles, components having an aromatic ring skeleton derived from PET and PBT are particularly effective in improving the mechanical strength of the resin particles.
[0057] Among these, a component with a smaller number of carbon atoms derived from the aliphatic diol is more preferable in terms of improving the mechanical strength of the resin particles, and the PET-derived component is particularly preferred. There are no particular restrictions on the weight-average molecular weight (Mw) of the PET and / or PBT, and it can be appropriately selected depending on the purpose, but 30,000 to 100,000 is preferred.
[0058] From an environmental standpoint, it is preferable that the monomer units derived from PET and / or PBT that may be included in the first resin are derived from recycled resin. In this specification, recycled resin refers to resin that has been recycled or was scheduled for disposal, rather than newly synthesized resin.
[0059] <Method for measuring the percentage of environmentally friendly components in resin particles or toner> -Method for measuring environmentally friendly component ratio- There are no particular limitations on the analytical and calculation methods for the content of plant-derived alcohol monomer units and PET or PBT-derived monomer units in the resin particles or toner of the present invention, and methods can be appropriately selected from known methods. For example, the mass ratio or molar ratio of the constituent components of the resin particles or toner can be calculated by separating them from the resin particles by gel permeation chromatography (GPC) or the like, and then applying the analytical methods described below to each separated component. Quantitative analysis is also possible by estimating the main constituent components from the soft decomposition of ester bonds in the resin structure by methylation using gas chromatography-mass spectrometry (GC / MS) at 300°C with a reaction reagent (10% tetramethylammonium hydroxide (TMAH) / methanol solution), and then drawing a calibration curve of total ion current chromatogram (TICC) intensity.
[0060] In this specification, monomer units derived from PET and / or PBT, preferably recycled PET and / or recycled PBT, and components containing the aforementioned plant-derived monomer units may be collectively referred to as "environmentally friendly components" or "recycled resins." Furthermore, the ratio of the total content of the aforementioned "environmentally friendly components" or "recycled resins" in resin particles or toner may be referred to as the "environmentally friendly component ratio" or "environmentally friendly ratio."
[0061] The aforementioned environmentally friendly component can be separated from the resin particles of the present invention as a chloroform-soluble component. The chloroform-soluble portion of the resin particles can be obtained as follows. One g of the resin particles is placed in 100 mL of chloroform, and under conditions of 25°C, the solution is obtained by stirring for 30 minutes until the soluble components are dissolved. This solution is filtered through a membrane filter with a mesh size of 0.2 μm to obtain the chloroform-soluble components in the resin particles.
[0062] The chloroform-soluble components obtained by the above method are dissolved in chloroform to prepare a sample for GPC measurement and injected into the GPC. A fraction collector is placed at the eluate outlet of the GPC, and the eluate is separated at predetermined count intervals (fractions corresponding to the desired molecular weight portion of the total integral of the elution curve are separated together), and eluate is obtained at intervals of 5% area from the start of elution (rise of the curve). Next, each eluate is concentrated and dried using an evaporator or the like, and then 30 mg of the sample is dissolved in 1 mL of deuterated chloroform to obtain the solid components, and 0.05 volume% of tetramethylsilane (TMS) is added as a reference substance. The obtained solution is packed into a 5 mm diameter glass tube for nuclear magnetic resonance (NMR) spectroscopy, and a nuclear magnetic resonance spectrometer (e.g., JNM-AL400, manufactured by JEOL Ltd.) is used to perform 128 integrations at a temperature of 23°C to 25°C to obtain a spectrum. From the peak integration ratio of the obtained spectrum, the monomer composition and constituent ratio of each resin contained in the resin particles in the eluted components can be determined.
[0063] Alternatively, after concentrating the eluate, hydrolysis can be performed using sodium hydroxide or the like, and the constituent monomer ratios can be calculated by qualitatively and quantitatively analyzing the decomposition products using high-performance liquid chromatography (HPLC).
[0064] The recycled resin that can be used in the first resin is preferably a polyester resin, and the polyester resin contained in the recycled resin preferably contains monomer units derived from recycled PET and / or PBT. The recycled resin is preferably, for example, a recycled product processed into flakes, and is preferably a recycled product using PET and / or PBT processed into flakes, and has a weight-average molecular weight (Mw) of 30,000 to 100,000. Furthermore, recycled PET and / or PBT, which are recycled resins, are not limited by their molecular weight distribution, composition, manufacturing method, or form of use, and can be appropriately selected according to the purpose.
[0065] Furthermore, the recycled resin, polyester resin, preferably PET and / or PBT, is not limited to recycled products (hereinafter sometimes referred to as "recycled resin"), and can be appropriately selected according to the purpose, and off-spec fiber scraps or pellets that do not meet the specifications for making a product may also be used. Furthermore, by adjusting the ratio of recycled resin, preferably recycled PET and / or PBT, introduced during polyester resin synthesis, the environmental friendliness ratio and quality of the toner when resin particles are used in the toner can be adjusted.
[0066] When the first resin contains PET and / or PBT-derived components, the PET and / or PBT content is preferably 70% by mass or less, more preferably 50% by mass or less, and even more preferably 30% by mass or less, based on 100% by mass of the first resin. If the amount of PET and / or PBT contained in the first resin is 70% by mass or less relative to 100% by mass of the first resin, it is advantageous in that the particle size distribution is improved.
[0067] -Crystalline resin- The first resin preferably contains a crystalline resin to improve low-temperature fixation. Crystalline resins are not particularly limited as long as they possess crystalline properties, and can be appropriately selected according to the purpose.
[0068] Examples of crystalline resins include polyester resins, polyurethane resins, polyurea resins, polyamide resins, polyether resins, vinyl resins, and modified crystalline resins. These may be used individually or in combination of two or more types.
[0069] The crystalline polyester resin can be obtained from a polyhydric alcohol and a polyhydric acid or its derivative, such as a polyhydric carboxylic acid, a polyhydric carboxylic acid anhydride, or a polyhydric carboxylic acid ester.
[0070] In this specification, modified polyester resins, such as prepolymers, and resins obtained by crosslinking and / or stretching the prepolymer are not considered crystalline polyester resins in this embodiment.
[0071] The polyhydric alcohols that can be used in the crystalline resin are not particularly limited and can be appropriately selected depending on the purpose, and examples include diols and alcohols with a hydride of three or higher.
[0072] Examples of diols that can be used in the crystalline resin include saturated aliphatic diols. Examples of saturated aliphatic diols include linear saturated aliphatic diols and branched saturated aliphatic diols, but among these, linear saturated aliphatic diols are preferred, and linear saturated aliphatic diols having 2 to 12 carbon atoms are more preferred.
[0073] If the saturated aliphatic diol that can be used in the crystalline resin is of the linear type, it is possible to suppress the decrease in the crystallinity of the crystalline polyester resin and the decrease in the melting point. Furthermore, when the saturated aliphatic diol has 2 to 12 carbon atoms, practical materials are readily available.
[0074] Examples of saturated aliphatic diols that can be used in the crystalline resin include ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 1,13-tridecanediol, 1,14-tetradecanediol, 1,18-octadecanediol, and 1,14-eicosandecanediol.
[0075] Among these, ethylene glycol, 1,4-butanediol, 1,6-hexanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, and 1,12-dodecanediol are preferred due to their high crystallinity and excellent sharp-melt properties in crystalline polyester resins.
[0076] Examples of trivalent or higher alcohols that can be used in the aforementioned crystalline resin include glycerin, trimethylolethane, trimethylolpropane, and pentaerythritol. These may be used individually or in combination of two or more.
[0077] The polycarboxylic acid that can be used in the crystalline resin is not particularly limited and can be appropriately selected depending on the purpose. Examples of polycarboxylic acids include divalent carboxylic acids and trivalent or higher carboxylic acids.
[0078] Examples of divalent carboxylic acids that can be used in the crystalline resin include saturated aliphatic dicarboxylic acids such as oxalic acid, succinic acid, glutaric acid, adipic acid, superiric acid, azelaic acid, sebacic acid, 1,9-nonanedicarboxylic acid, 1,10-decanedicarboxylic acid, 1,12-dodecanedicarboxylic acid, 1,14-tetradecanedicarboxylic acid, and 1,18-octadecanedicarboxylic acid; aromatic dicarboxylic acids such as phthalic acid, isophthalic acid, terephthalic acid, naphthalene-2,6-dicarboxylic acid, malonic acid, and mesaconic acid; and their anhydrides and lower (1-3 carbon atoms) alkyl esters.
[0079] Among these, from the perspective of carbon neutrality, saturated aliphatic materials with 12 or fewer carbon atoms derived from plants are preferred.
[0080] Examples of trivalent or higher carboxylic acids that can be used in the crystalline resin include 1,2,4-benzenetricarboxylic acid, 1,2,5-benzenetricarboxylic acid, 1,2,4-naphthalentricarboxylic acid, and their anhydrides and lower (C1-C3) alkyl esters. These may be used individually or in combination of two or more.
[0081] The crystalline polyester resin that can be used in the aforementioned crystalline resin is preferably composed of a linear saturated aliphatic dicarboxylic acid having 4 to 12 carbon atoms and a linear saturated aliphatic diol having 2 to 12 carbon atoms. This results in high crystallinity and excellent sharp melt properties, thus enabling excellent low-temperature fixation.
[0082] Furthermore, as a method for controlling the crystallinity and softening point of crystalline polyester resins that can be used in the aforementioned crystalline resins, one can design and use nonlinear polyesters that have been subjected to condensation polymerization by adding a trivalent or higher polyhydric alcohol such as glycerin to the alcohol component, or a trivalent or higher polyhydric carboxylic acid such as trimellitic anhydride to the acid component.
[0083] The molecular structure of the crystalline polyester resin that can be used in the aforementioned crystalline resin can be confirmed by NMR measurements in solution or solid state, as well as by X-ray diffraction, GC / MS, LC / MS, IR measurements, etc.
[0084] For simplicity, in the infrared absorption spectrum, 965±10 cm⁻¹ -1 Alternatively, 990±10cm -1 Examples include those exhibiting absorption based on δCH (out-of-plane bending vibration) of olefins.
[0085] Regarding the molecular weight of the crystalline polyester resin that can be used in the aforementioned crystalline resin, from the viewpoint that a sharp molecular weight distribution and low molecular weight result in excellent low-temperature fixation, and that a large amount of low molecular weight components worsens heat resistance and storage performance, it is preferable that the molecular weight distribution of the soluble components of o-dichlorobenzene, as determined by GPC, shows a molecular weight distribution graph with log(M) on the x-axis and mass% on the y-axis, with the peak position in the range of 3.5 to 4.0, the full width at half maximum of the peak being 1.5 or less, a weight-average molecular weight (Mw) of 3,000 to 30,000, a number-average molecular weight (Mn) of 1,000 to 10,000, and an Mw / Mn ratio of 1 to 10.
[0086] Furthermore, it is preferable that the molecular weight of the crystalline polyester resin that can be used in the crystalline resin is 5,000 to 15,000 in weight-average molecular weight (Mw), 2,000 to 10,000 in number-average molecular weight (Mn), and Mw / Mn is 1 to 5.
[0087] The acid value of the crystalline polyester resin is preferably 5 mg KOH / g or higher when the resin particles are used in toner, in order to achieve the desired low-temperature fixation from the viewpoint of the affinity between the paper and the resin. Furthermore, for the production of fine particles by the phase inversion emulsification method, it is more preferable that the acid value be 7 mg KOH / g or higher.
[0088] On the other hand, to improve hot offset properties, it is preferable that the KOH content be 45 mg / g or less. Furthermore, regarding the hydroxyl value of the crystalline polymer, in order to achieve the required low-temperature fixation properties and good charging characteristics, it is preferable that it be 0 to 50 mg KOH / g, more preferably 5 to 50 mg KOH / g.
[0089] <<shell>> The shell is the outer shell portion that covers at least a portion of the surface of the core in the resin particles of the core-shell structure. Furthermore, the shell layer of the resin particles of the present invention may contain a second resin, and the shell layer may contain some or all of the resin contained in the core, or some or all of the resin contained in the core may be contained as domains or domain particles. The second resin that may be included in the shell is an example of the resin in this embodiment.
[0090] -Second resin- The second resin may be contained within the shell of the core-shell structure and contains 2 mol% to 30 mol% of plant-derived alcohol monomer units per 100 mol% of alcohol monomer units.
[0091] The second resin preferably contains an amorphous resin, and the amorphous resin that may be included in the second resin is the same as the amorphous resin that may be included in the first resin.
[0092] Furthermore, the second resin may or may not contain polyester-derived monomer units derived from PET and / or PBT, but it is preferable to contain monomer units derived from PET and / or PBT in terms of heat resistance and filming resistance. The monomer units derived from polyester that may be included in the second resin are preferably monomer units derived from PET and / or PBT, and the monomer units derived from PET and / or PBT that may be included in the second resin are the same as those derived from PET and / or PBT that may be included in the first resin.
[0093] The content of monomer units derived from PET and / or PBT that may be contained in the second resin is preferably 40% by mass or less, more preferably 30% by mass or less, and even more preferably 20% by mass or less, based on 100% by mass of the second resin. If the content of monomer units derived from PET and / or PBT in the second resin is 40% by mass or less of 100% by mass of the second resin, the strength of the resin particles can be supplemented, thereby providing resin particles that yield toner with excellent strength and low-temperature fixability while reducing environmental impact.
[0094] Furthermore, the second resin preferably contains a crystalline resin to improve low-temperature fixation. The crystalline resin that may be included in the second resin is the same as the crystalline resin that may be included in the first resin.
[0095] Furthermore, the second resin preferably includes a non-plant-derived resin (including monomer units), and the non-plant-derived resin (non-plant-derived resin) preferably includes, for example, monomer units produced from petroleum. By including non-plant-derived resins and monomer units in the second resin, the location of components containing plant-derived alcohol monomer units and PET and / or PBT-derived monomer units in the resin can be controlled. This reduces the amount of resin containing plant-derived alcohol monomer units and PET and / or PBT-derived monomer units on the surface of the resin particles, thereby suppressing a decrease in strength and preventing a decrease in the durability and heat resistance of the resin particles.
[0096] The content of non-plant-derived resin in the second resin is preferably 50% to 90% by mass, and more preferably 70% to 80% by mass, relative to 100% by mass of the second resin. A content of 50% to 90% by mass allows for both reduced environmental impact and heat-resistant storage.
[0097] <<Composition of the shell layer>> In the resin particles of the present invention, when the shell layer is divided into 10 equal parts in the diametrical direction, the outermost resin has a signal peak intensity that is 5 times or more greater than the sum of the signal peak intensity of plant-derived alcohol monomer units obtained by measurement with nano-IR (also referred to as "AMF-IR") and the signal peak intensity of monomer units derived from at least one of PET and PBT. There is no upper limit as long as the resin particles of the present invention can be manufactured, but generally, a value of 20 times or less, or 10 times or less, makes it easier to manufacture the resin particles.
[0098] The term "diameter direction" refers to the particle size direction of the representative diameter (volume particle size, etc.) of the resin particles.
[0099] In the outermost resin when the shell layer is divided into 10 equal parts in the diametrical direction, if the intensity of non-plant-derived components is less than 5 times the sum of the signal peak intensity of plant-derived alcohol monomer units obtained by nano IR measurement and the signal peak intensity of monomer units derived from at least one of PET and PBT, the resin will aggregate at high temperatures.
[0100] In the core-shell structure, when the shell layer is divided into 10 equal parts in the diametrical direction, the outermost resin should have a signal peak intensity of non-plant-derived monomer units that is 5 times or more greater than the sum of the signal peak intensity of plant-derived alcohol monomer units obtained by nano IR measurement and the signal peak intensity of monomer units derived from at least one of PET and PBT. It is also acceptable for either the signal peak intensity of plant-derived alcohol monomer units obtained by nano IR measurement or the signal peak intensity of monomer units derived from at least one of PET and PBT to be 0.
[0101] The shell layer in the resin particles of the present invention preferably contains domain particles, and the domain particles may contain the resin contained in the core, or they may contain the first resin.
[0102] Conventionally, the shell layer in resin particles for toner was a uniform layer. However, in the resin particle manufacturing process, by attaching resin particles with a core-shell structure that may contain a first resin and a second resin to resin particles containing a first resin core, it is possible to provide resin particles or toner containing domains or domain particles in the shell layer of the present invention. Such resin particles or toners require less manufacturing energy and auxiliary materials, and even when using plant-derived resins, they can provide toners with excellent heat resistance and storage properties. The domains or domain particles can be observed using a transmission electron microscope (TEM).
[0103] There are no particular restrictions on the method for confirming the composition of the shell layer, and it can be appropriately selected depending on the purpose. For example, it can be confirmed by surface (shell layer) composition analysis using nano IR. By using an analytical technique that achieves nanoscale resolution by combining nano IR atomic force microscopy (AFM) and IR, the composition can be determined by obtaining the IR spectrum of the surface layer (shell layer) of the resin particles or toner. Specifically, the resin particles are embedded in epoxy resin (S-31, manufactured by DEVCON) and cured. A cross-section is then made using a knife, and the resin particles or toner are cut to a thickness of approximately 100 nm using an ultrasonic ultramicrotome (Leica EM UC7, manufactured by Leica) to produce ultrathin sections of the resin particles or toner. The prepared ultrathin sections of toner are collected on a substrate (ZnS), and the measurement area (shell layer) is measured using AFM-IR spectroscopy with a nanoscale infrared spectroscopy system (e.g., nanoIR2, manufactured by Anasys Instruments). The measurement range is 1,900 cm². -1 From 910cm -1 The resolution is 2cm. -1 The resulting AFM-IR absorption spectrum allows for the analysis of the chemical structure of the measurement site (shell layer). Therefore, this analysis allows us to confirm the compositional structure of the surface layer (shell layer). Furthermore, by designating the measurement location as the core layer, the chemical structure of the core layer can also be analyzed.
[0104] <Shell thickness> The shell thickness can be measured based on transmission electron microscope (TEM) images of the cross-section of an ultrathin section of toner.
[0105] The shell thickness shall be the value obtained by calculating from the following formula. Shell thickness = Average equivalent diameter of resin particles in the core-shell structure / Average equivalent diameter of the core
[0106] The shell thickness is not limited and can be selected as appropriate, but for example, the shell thickness defined by the ratio of the average circular equivalent diameter of the resin particles to the average circular equivalent diameter of the core (a value calculated by the above formula) is preferably 1.005 or more and 1.5 or less, more preferably 1.01 or more and 1.3 or less, and even more preferably 1.03 or more and 1.1 or less. By adjusting the shell thickness of the resin particles to be between 1.005 and 1.5, it is possible to obtain resin particles that reduce environmental impact without compromising toner durability.
[0107] There are no particular restrictions on the coverage rate of the shell layer on the surface of the core layer, and it can be appropriately selected depending on the purpose, but 50% to 100% is preferred, and 80% to 100% is more preferred. A coverage rate of 100% means that the entire surface area of the core layer in the resin particles is covered with the shell layer. The coverage rate (%) of the core layer surface by the shell layer can be calculated by the following formula (2). Coverage rate (%) = (Area of covered region) / (Total surface area of resin particles) × 100 ... Equation (2) In formula (2) above, "total surface area of resin particles" means the sum of the area of the covered region and the exposed core layer area, "area of the covered region" means the area of the total surface area of resin particles in which the core layer is covered by the shell layer, and "exposed core layer area" means the area of the total surface area of resin particles in which the core layer is not covered by the shell layer.
[0108] There are no particular limitations on the method for confirming that the resin particles have a core-shell structure, and a suitable method can be selected depending on the purpose. For example, the resin particles can be embedded in epoxy resin (S-31, manufactured by DEVCON) and cured, then cross-sectioned with a knife, and excised to a thickness of approximately 100 nm using an ultrasonic ultramicrotome (Leica EM UC7, manufactured by Leica) to prepare ultrathin sections of the resin particles. The prepared ultrathin sections of the toner are gas-exposed with ruthenium tetroxide (RuO4) to distinguish and stain the shell and core. The gas exposure time can be adjusted as appropriate depending on the contrast during observation. Subsequently, confirmation can be made by observing a cross-sectional image of the resin particles using a transmission electron microscope (TEM) (H-7500, manufactured by Hitachi High-Tech Corporation) at an accelerating voltage of 120 kV.
[0109] Furthermore, in the TEM images observed using the method described above, the core layer coverage area on the surface of the resin particle (the area in the resin particle where the core layer is covered by the shell layer) and the exposed core layer area (the area in the resin particle where the core layer is not covered by the shell layer) can be distinguished by the difference in brightness values. Therefore, by performing binarization processing on the TEM images observed using the method described above using image processing software, the shell layer can be identified by its contrast ratio, and the thickness of the shell layer can be measured.
[0110] Image-J, Image-Pro Plus, etc., can be used as the aforementioned image processing software. The method for calculating the average thickness of the shell layer using Image-J is as follows. (1) Use Straight Line to draw a straight line that traces the scale. Use Analyze's Set Scale to set its actual length and units. (2) The outer circumference of a single resin particle in the cross-sectional image of the resin particle is enclosed by freehand sections to create "region 1". (3) The outer periphery of the region excluding the shell layer in the cross-sectional image of one resin particle (i.e., the boundary between the shell layer and the core layer) is enclosed with freehand sections to create "region 2". (4) Determine the center of mass of "region 1" using Analyze. (5) Using a proprietary plugin, a straight line is drawn from the outer perimeter of "region 1," that is, from the coordinates obtained by dividing the line that encloses the outer perimeter of one resin particle in (2) with Freehand-sections into 100 equally spaced sections, toward the center of gravity of the resin particle determined in (4). (6) The length obtained by subtracting the length passing through "Region 2" from the length of each of the 100 straight lines created in (5) above is calculated using the straight lines that trace the scale created in (1) above, and the average of the 100 values is taken as the thickness of the shell layer of one resin particle. (7) Perform the operations described in (2) to (6) above for 50 resin particles and calculate the average thickness of the shell layer of the 50 resin particles or toner. This average value is taken as the average thickness of the shell layer in the present invention.
[0111] Furthermore, the method for calculating the coverage rate of the shell layer using Image-J is as follows. (1) Trace the portion of the outer periphery of a single resin particle covered by the shell layer in the cross-sectional image of the resin particle using Freehand Line, and measure the length of the traced line using Analyze. This length is defined as "length 1". (2) Trace the outer circumference of one resin particle in the cross-sectional image of the resin particle using Freehand Line, and measure the length of the traced line using Analyze. This length shall be "Length 2". (3) Calculate (length 1 / length 2) × 100 and use this as the coverage rate of the shell layer of one resin particle. (4) Perform the operations described in (1) to (3) above for 50 resin particles and calculate the average value of the coating rate by the shell layer of the 50 resin particles or toner. This average value is taken as the coating rate by the shell layer in the present invention.
[0112] The shell thickness value is preferably obtained using image processing software, but is not limited to the above-mentioned transmission microscope, image analysis device, and software, as long as similar analysis results can be obtained. The above average circle equivalent diameter can be calculated by binarization processing using image editing software.
[0113] - Observation and measurement of resin particles or toner cross-sections using TEM - The prepared resin particles or toner can be embedded in epoxy resin and cured, and then ultrathin sections (approximately 100 nm thick) of the resin particles or toner can be prepared using an ultramicrotome (Leica ULTRACUT UCT, using a diamond knife), allowing for observation of the cross-section of the resin particles or toner.
[0114] The core and shell layers can be distinguished by gas exposure of the sample with ruthenium tetroxide, osmium tetroxide, or another staining agent. The exposure time can be adjusted as appropriate depending on the contrast during observation. Subsequently, the sample can be observed using a transmission electron microscope (e.g., JEM-2100, JEOL) at an accelerating voltage of 100kV.
[0115] Furthermore, compositional contrast can be imparted by other means such as selective etching. After such pretreatment, the core layer and shell layer can be evaluated by observation with a transmission microscope, and if domain particles are present in the shell layer, those domain particles can be identified.
[0116] The observed cross-sectional images can be processed using commercially available image processing software (e.g., Image-J, Image-Pro Plus) to perform binarization and other operations to calculate the average equivalent diameter of the resin particles or toner in the core-shell structure and the average equivalent diameter of the core. By observing multiple toner cross-sections, the average equivalent diameter can be determined.
[0117] In this specification, the average equivalent diameter of resin particles or toner can be calculated by binarizing a cross-sectional image of the resin particles or toner observed with a transmission electron microscope (TEM) using image processing software. The shell thickness is represented by the value obtained by dividing the average equivalent circular diameter of the resin particles by the average equivalent circular diameter of the resin particles.
[0118] -Analysis of the resin composition of resin particles or the toner surface layer- The presence of plant-derived alcohol monomer units and PET and / or PBT-derived monomer units in the resin particles or toner surface can be confirmed by surface composition analysis using nano IR. By obtaining the IR spectrum of the resin particle surface using an analytical method that achieves nanoscale resolution by combining AFM and IR in nano IR, the compositional structure can be determined. This analysis can identify whether plant-derived alcohol monomer units or monomer units derived from PET and / or PBT are present on the surface of the shell layer. Furthermore, by analyzing the composition of the resin particles or the toner surface layer, the amount of plant-derived or PET and / or PBT-derived resin components in the surface layer of the shell layer can be analyzed. By analyzing the composition of resin particles or the toner surface using nano IR, it is possible to determine the ratio of the signal peak intensity of plant-derived alcohol monomer units, PET and PBT-derived monomer units, and non-plant-derived monomer units (excluding PET and PBT) obtained by nano IR measurement in the outermost resin when the shell layer of the resin particle is divided into 10 equal parts in the diametrical direction.
[0119] <Method for analyzing resin particles or toner components> Plant-derived alcohol monomer units, PET, and PBT contained in resin particles or toner can be analyzed using any method. For example, they can be separated from the toner by gel permeation chromatography (GPC), and then qualitatively analyzed using the analytical methods described below for each separated component.
[0120] Gas chromatography-mass spectrometry at 300°C using a reaction reagent (10% Tetramethyl ammonium hydroxide (TMAH) / Methanol solution) allows for the estimation of the main components of the resin structure by observing the soft decomposition of ester bonds through methylation.
[0121] <<Method for measuring melting point and glass transition temperature (Tg)>> In this specification, the melting point and glass transition temperature (Tg) of each component can be measured, for example, using a DSC system (differential scanning calorimeter) (Q-200, manufactured by TA Instruments). Specifically, the melting point and glass transition temperature of the target sample can be measured by the following procedure. First, approximately 5.0 mg of the sample is placed in an aluminum sample container, which is then placed on a holder unit and set in an electric furnace. Next, under a nitrogen atmosphere, the sample is heated from -80°C to 150°C at a heating rate of 10°C / min (first heating pass). After that, it is cooled from 150°C to -80°C at a cooling rate of 10°C / min, and then heated again to 150°C at a heating rate of 10°C / min (second heating pass). During both the first and second heating passes, a differential scanning calorimeter (Q-200, TA Instruments Inc.) is used to measure the DSC curve. From the obtained DSC curves, the analysis program in the Q-200 system can be used to select the DSC curve for the first heating cycle and determine the glass transition temperature of the sample during the first heating cycle. Similarly, the DSC curve for the second heating cycle can be selected to determine the glass transition temperature of the sample during the second heating cycle. Furthermore, using the analysis program in the Q-200 system, the DSC curve obtained can be selected for the first heating cycle, and the endothermic peak top temperature of the sample during the first heating cycle can be determined as the melting point. Similarly, the DSC curve obtained for the second heating cycle can be selected, and the endothermic peak top temperature of the sample during the second heating cycle can be determined as the melting point. In this specification, unless otherwise specified, the glass transition temperature and melting point of amorphous polyester resin and other components such as the mold release agent shall be determined by the endothermic peak top temperature at the second heating stage as the melting point of each sample, and the Tg at the second heating stage as the Tg of each sample.
[0122] <Other ingredients> The resin particles of the present invention may optionally contain, as other components besides the first resin, the second resin, and the crystalline polyester resin described above, a colorant, a prepolymer, a charge control agent, a wax (release agent), a fluidity enhancer, a cleaning property enhancer, a magnetic material, and a shape-forming agent.
[0123] -Coloring agent- The coloring agent is not particularly limited, and known dyes and pigments can be used and selected as appropriate depending on the purpose. Examples of colorants include carbon black, nigrosine dye, iron black, naphthol yellow S, Hansa yellow (10G, 5G, G), cadmium yellow, yellow iron oxide, yellow ochre, yellow lead, titanium yellow, polyazo yellow, oil yellow, Hansa yellow (GR, A, RN, R), pigment yellow L, benzidine yellow (G, GR), permanent yellow (NCG), Vulcan fast yellow (5G, R), tartrazine lake, quinoline yellow lake, anthrazan yellow BGL, isoindolinone yellow, red iron oxide, red lead, red lead, ka Dominum Red, Cadmium Mercury Red, Antimony Vermilion, Permanent Red 4R, Para Red, Faise Red, Parachlor-Orthonitroaniline Red, Risol Fast Scarlet G, Brilliant Fast Scarlet, Brilliant Carmine BS, Permanent Red (F2R, F4R, FRL, FRLL, F4RH), Fast Scarlet VD, Belkan Fast Rubin B, Brilliant Scarlet G, Risol Rubin GX, Permanent Red F5R, Brilliant Carmine 6B, Pogment Scarlet 3B, Vol Do 5B, Toluidine Maroon, Permanent Bordeaux F2K, Helio Bordeaux BL, Bordeaux 10B, Bon Maroon Light, Bon Maroon Medium, Eosin Lake, Rhodamine Lake B, Rhodamine Lake Y, Alizarin Lake, Thioindigo Red B, Thioindigo Maroon, Oil Red, Quinacridone Red, Pyrazolone Red, Polyazo Red, Chrome Vermilion, Benzidine Orange, Perinon Orange, Oil Orange, Cobalt Blue, Cerulean Blue, Alkali Blue Lake, Peacock Blue Lake, Victoria Blue -Ki, metal-free phthalocyanine blue, phthalocyanine blue, fast sky blue, indanthrene blue (RS, BC), indigo, ultramarine, navy blue, anthraquinone blue, fast violet B, methyl violet lake, cobalt purple, manganese purple, dioxane violet, anthraquinone violet, chrome green, zinc green, chromium oxide, pyridian, emerald green, pigment green B, naphthol green B, green gold, acid green lake, malachite green lake, phthalocyanine green,Examples include anthraquinone green, titanium dioxide, zinc oxide, lithobone, and mixtures thereof.
[0124] These colorants may be used individually or in combination of two or more.
[0125] The amount of colorant is not particularly limited and can be appropriately selected depending on the purpose. For example, the amount of colorant is preferably 1% to 15% by mass, and more preferably 3% to 10% by mass, per 100% by mass of resin particles.
[0126] The colorants can also be used as a masterbatch compounded with resin.
[0127] -Prepolymer- Examples of prepolymers (reactive precursors) include polyesters that have groups that can react with active hydrogen groups.
[0128] Examples of groups that can react with active hydrogen groups include isocyanate groups, epoxy groups, carboxylic acids, and acid chloride groups. Among these, isocyanate groups are preferred because they can introduce urethane or urea bonds into amorphous polyester resins.
[0129] The reactive precursor may have a branched structure conferred by at least one of a trivalent or higher alcohol and a trivalent or higher carboxylic acid.
[0130] Examples of polyester resins containing isocyanate groups include reaction products of polyester resins having active hydrogen groups and polyisocyanates.
[0131] Polyester resins having active hydrogen groups can be obtained, for example, by polycondensation of a diol, a dicarboxylic acid, and at least one of a trivalent or higher alcohol and a trivalent or higher carboxylic acid. The trivalent or higher alcohol and the trivalent or higher carboxylic acid impart a branched structure to the polyester resin containing isocyanate groups.
[0132] Examples of diols include aliphatic diols such as ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,4-butanediol, 2-methyl-1,3-propanediol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, 1,8-octanediol, 1,10-decanediol, and 1,12-dodecanediol; diethylene glycol, triethylene glycol, dipropylene glycol, polyethylene glycol, polypropylene glycol, and polytetramethyl Examples include diols having oxyalkylene groups such as ethylene glycol; alicyclic diols such as 1,4-cyclohexanedimethanol and hydrogenated bisphenol A; alicyclic diols to which alkylene oxides such as ethylene oxide, propylene oxide, and butylene oxide have been added; bisphenols such as bisphenol A, bisphenol F, and bisphenol S; and alkylene oxide adducts of bisphenols to which alkylene oxides such as ethylene oxide, propylene oxide, and butylene oxide have been added.
[0133] Among these, from the viewpoint of controlling the glass transition temperature of the polyester resin to 20°C or below, it is preferable to use aliphatic diols having 3 to 10 carbon atoms, such as 1,2-propylene glycol, 1,3-propylene glycol, 1,4-butanediol, 2-methyl-1,3-propanediol, 1,5-pentanediol, and 3-methyl-1,5-pentanediol, and it is more preferable to use them in an alcohol component of 50 mol% or more in the resin. These diols may be used individually or in combination of two or more.
[0134] The polyester resin is preferably amorphous, and sterically hindering the resin chain reduces the melt viscosity during fixing, making it easier to achieve low-temperature fixing properties. For this reason, the main chain of the aliphatic diol is preferably structured as shown in the following general formula (3).
[0135] [ka] [In the formula, R1 and R2 each independently represent a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, and n represents an odd number from 3 to 9. However, in n repeating units, R1 and R2 may be the same or different.]
[0136] Here, the main chain of an aliphatic diol refers to the carbon chain connecting the two hydroxyl groups of the aliphatic diol in the shortest possible number of carbon atoms. When the number of carbon atoms in the main chain is odd, it is preferable because the crystallinity decreases due to the oddness. Furthermore, when there is at least one alkyl group with 1 to 3 carbon atoms in the side chain, it is more preferable because the interaction energy between the main chain molecules decreases due to the stericity.
[0137] Examples of dicarboxylic acids include aliphatic dicarboxylic acids such as succinic acid, adipic acid, sebacic acid, dodecanedioic acid, maleic acid, and fumaric acid; and aromatic dicarboxylic acids such as phthalic acid, isophthalic acid, terephthalic acid, and naphthalenedicarboxylic acid. Anhydrides, lower (1-3 carbon atom) alkyl esters, and halides of these dicarboxylic acids may also be used.
[0138] Among these, aliphatic dicarboxylic acids having 4 to 12 carbon atoms are preferred from the viewpoint of controlling the Tg of the polyester resin to 20°C or below, and it is more preferable to use them in an amount of 50% by mass or more of the carboxylic acid component in the resin. These dicarboxylic acids may be used individually or in combination of two or more.
[0139] Examples of trivalent or higher alcohols include trivalent or higher aliphatic alcohols such as glycerin, trimethylolethane, trimethylolpropane, pentaerythritol, and sorbitol; trivalent or higher polyphenols such as trisphenol PA, phenol novolac, and cresol novolac; and alkylene oxide adducts of trivalent or higher polyphenols, such as those obtained by adding alkylene oxides such as ethylene oxide, propylene oxide, and butylene oxide to trivalent or higher polyphenols.
[0140] Examples of trivalent or higher carboxylic acids include trivalent or higher aromatic carboxylic acids, with trimellitic acid and pyromellitic acid, which have 9 to 20 carbon atoms, being particularly preferred. Alternatively, their anhydrides, lower (1 to 3 carbon atoms) alkyl esters, and halides may also be used.
[0141] Polyisocyanates are not particularly limited and can be selected as appropriate depending on the purpose; for example, diisocyanates and isocyanates with a valentity of 3 or higher can be used.
[0142] Specifically, polyisocyanates include 1,3- and / or 1,4-phenylenediisocyanate, 2,4- and / or 2,6-tolylenediisocyanate (TDI), crude TDI, 2,4'- and / or 4,4'-diphenylmethane diisocyanate (MDI), crude MDI [a phosgenate of crude diaminophenylmethane (a condensation product of formaldehyde and an aromatic amine (aniline) or a mixture thereof; a mixture of diaminodiphenylmethane and a small amount (e.g., 5-20% by mass) of a trifunctional or higher polyamine): poly Aromatic diisocyanates such as allyl polyisocyanate (PAPI), 1,5-naphthylene diisocyanate, 4,4',4"-triphenylmethane triisocyanate, m- and p-isocyanatophenylsulfonyl isocyanates; ethylene diisocyanate, tetramethylene diisocyanate, hexamethylene diisocyanate (HDI), dodecamethylene diisocyanate, 1,6,11-undecane triisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, lysine diisocyanate, Aliphatic diisocyanates such as 2,6-diisocyanatomethyl caproate, bis(2-isocyanatoethyl) fumarate, bis(2-isocyanatoethyl) carbonate, 2-isocyanatoethyl-2,6-diisocyanatohexanoate; isophorone diisocyanate (IPDI), dicyclohexylmethane-4,4'-diisocyanate (hydrogenated MDI), cyclohexylene diisocyanate, methylcyclohexylene diisocyanate (hydrogenated TDI), bis(2-isocyanatoethyl)-4-cyclohexene-1, Examples include alicyclic diisocyanates such as 2-dicarboxylate and 2,5- and 2,6-norbornane diisocyanates; aromatic aliphatic diisocyanates such as m- and p-xylylene diisocyanates (XDI) and α,α,α',α'-tetramethylxylylene diisocyanate (TMXDI); polyisocyanates with a valency of 3 or higher, such as lysine triisocyanate and diisocyanate-modified alcohols with a valency of 3 or higher; and modified products of these isocyanates. These may be used individually or in combination of two or more.
[0143] Examples of modified isocyanates include those containing urethane groups, carbodiimide groups, allophanate groups, urea groups, biuret groups, uretodione groups, uretoimine groups, isocyanurate groups, and oxazolidone groups.
[0144] -Static control agent- The charge control agent is not particularly limited, and all known agents can be used and selected as appropriate depending on the purpose. Examples of charge control agents include nigrosine dyes, triphenylmethane dyes, chromium-containing metal complex dyes, molybdate chelate pigments, rhodamine dyes, alkoxyamines, quaternary ammonium salts (including fluorine-modified quaternary ammonium salts), alkylamides, elemental or compound phosphorus, elemental or compound tungsten, fluorine-based surfactants, metal salicylic acid salts, and metal salts of salicylic acid derivatives.
[0145] Specifically, the charge control agents include Bontron 03 (a nigrosine-based dye), Bontron P-51 (a quaternary ammonium salt), Bontron S-34 (a metal-containing azo dye), E-82 (an oxynaphthoic acid-based metal complex), E-84 (a salicylic acid-based metal complex), and E-89 (a phenolic condensate) (all manufactured by Orient Chemical Industry Co., Ltd.), TP-302 and TP-415 (quaternary ammonium salt molybdenum complexes) (both manufactured by Hodogaya Chemical Co., Ltd.), Copy Charge PSY VP2038 (a quaternary ammonium salt), Copy Blue PR (a triphenylmethane derivative), Copy Charge NEG VP2036 (a quaternary ammonium salt), and Copy Charge NX Examples include VP434 (manufactured by Hoechst), LRA-901, the boron complex LR-147 (manufactured by Nippon Carlit Co., Ltd.), copper phthalocyanine, perylene, quinacridone, azo pigments, and other polymer compounds having functional groups such as sulfonic acid groups, carboxyl groups, and quaternary ammonium salts.
[0146] The charge control agent should be used in an amount that exhibits performance without hindering fixation, and is preferably present in 0.5 to 5% by mass in the resin particles, and more preferably in 0.8 to 3% by mass.
[0147] -Wax (release agent)- The wax is not particularly limited and can be selected as appropriate depending on the purpose, but a low-melting-point release agent with a melting point of 50°C to 120°C is preferred. When a low-melting-point release agent is dispersed with the resin, it works effectively as a release agent between the fixing roller and the toner interface when resin particles are used as toner, thereby providing good hot offset even in an oil-free (no release agent such as oil is applied to the fixing roller) environment.
[0148] Suitable release agents include, for example, waxes and other similar substances. Examples of waxes and other similar substances include plant-based waxes such as carnauba wax, cotton wax, wood wax, and rice wax; animal-based waxes such as beeswax and lanolin; mineral-based waxes such as ozokelite and cerucine; and petroleum waxes such as paraffin, microcrystalline, and petrolatum.
[0149] In addition to these natural waxes, other examples include synthetic hydrocarbon waxes such as Fischer-Tropsch wax and polyethylene wax; and synthetic waxes such as esters, ketones, and ethers.
[0150] Furthermore, fatty acid amides such as 12-hydroxystearic acid amide, stearic acid amide, phthalic anhydride, and chlorinated hydrocarbons may be used; homopolymers or copolymers of polyacrylates such as poly-n-stearyl methacrylate and poly-n-lauryl methacrylate, which are low molecular weight crystalline polymer resins (for example, copolymers of n-stearyl acrylate and ethyl methacrylate); and crystalline polymers having long alkyl groups in their side chains may also be used. These may be used individually or in combination of two or more.
[0151] Among these waxes, plant-based waxes are preferred from a carbon neutrality perspective.
[0152] There are no particular restrictions on the melting point of the wax, and it can be appropriately selected depending on the purpose, but 50°C to 120°C is preferred, and 60°C to 90°C is more preferred. If the melting point is 50°C or higher, it is possible to prevent the wax from adversely affecting its heat resistance during storage, and if it is 120°C or lower, it is possible to effectively prevent the problem of cold offset occurring during fixing at low temperatures.
[0153] The melt viscosity of the wax is preferably 5 cps to 1,000 cps, and more preferably 10 cps to 100 cps, measured at a temperature 20°C higher than the melting point of the wax. If the melt viscosity is 5 cps or higher, a decrease in release properties can be prevented, and if it is 1,000 cps or lower, the effects of hot offset resistance and low-temperature fixing can be fully exhibited.
[0154] The wax content in the resin particles is not particularly limited and can be appropriately selected depending on the purpose, but it is preferably 0% by mass or more and 40% by mass or less, and more preferably 3% by mass or more and 30% by mass or less. When the content is 40% by mass or less, deterioration of toner fluidity can be prevented when the resin particles are used in toner.
[0155] -External additives- External additives are not particularly limited and can be selected as appropriate depending on the purpose. Examples of external additives include inorganic microparticles and polymer microparticles.
[0156] The primary particle size of the inorganic fine particles is preferably 5 nm to 2 μm, and particularly preferably 5 nm to 500 nm.
[0157] The specific surface area of inorganic nanoparticles calculated by the BET method is 20-500 m². 2 It is preferable that it be / g.
[0158] The proportion of inorganic fine particles used is preferably 0.01% by mass or more and 5% by mass or less relative to the resin particles.
[0159] Specific examples of inorganic fine particles include silica, alumina, titanium oxide, barium titanate, magnesium titanate, calcium titanate, strontium titanate, zinc oxide, tin oxide, silica sand, clay, mica, wollastonite, diatomaceous earth, chromium oxide, cerium oxide, pengala, antimony trioxide, magnesium oxide, zirconium oxide, barium sulfate, barium carbonate, calcium carbonate, silicon carbide, and silicon nitride.
[0160] Examples of polymer-based microparticles include polymer particles made from polystyrene, methacrylic acid esters, acrylic acid ester copolymers, silicon, benzoguanamine, nylon, and other polycondensation systems and thermosetting resins obtained by soap-free emulsion polymerization, suspension polymerization, or dispersion polymerization.
[0161] - Fluidity improver - Furthermore, a fluidity enhancer can be added to the resin particles of the present invention. Such a fluidity enhancer can be surface-treated to increase its hydrophobicity, preventing deterioration of fluidity and electrostatic properties even under high humidity conditions.
[0162] For example, preferred surface treatment agents include silane coupling agents, silylation agents, silane coupling agents having alkyl fluoride compounds, organic titanate coupling agents, aluminum coupling agents, silicone oil, and modified silicone oil.
[0163] -Cleaning performance enhancer- Examples of cleaning agents used to remove residual developer after transfer from the photoreceptor or primary transfer medium include fatty acid metal salts such as zinc stearate, calcium stearate, and stearic acid, as well as polymer microparticles produced by soap-free emulsion polymerization, such as polymethyl methacrylate microparticles and polystyrene microparticles.
[0164] The polymer fine particles preferably have a relatively narrow particle size distribution, with a volume-average particle size of 0.01 to 1 μm.
[0165] -Magnetic materials- There are no particular limitations on the magnetic material, and it can be appropriately selected depending on the purpose. Examples include iron powder, magnetite, or ferrite. These may be used individually or in combination of two or more. Among these, a white magnetic material is preferred in terms of color.
[0166] There are no particular restrictions on the content of the magnetic material, and it can be appropriately selected depending on the purpose, but it is preferably 20 parts by mass or more and 200 parts by mass or less, and more preferably 40 parts by mass or more and 150 parts by mass or less, per 100 parts by mass of the resin particles.
[0167] -Modifying agent- The aforementioned shape-modifying agent is added to modify the shape of the resin particles. There are no particular restrictions on the modifying agent, and it can be appropriately selected depending on the purpose, but it is preferable that it contains a layered inorganic mineral in which at least a portion of the interlayer ions of the layered inorganic mineral are modified with organic ions.
[0168] There are no particular limitations on the layered inorganic mineral in which at least a portion of the interlayer ions are modified with organic ions, and it can be appropriately selected according to the purpose. For example, a layered inorganic mineral having a basic smectite crystal structure modified with organic cations can be used. Smectite clay minerals have negatively charged layers, and cations exist between the layers to compensate for this. Interlayer compounds can be formed by ion exchange of these cations or adsorption of polar molecules. In addition, metal ions can be introduced by substituting some of the divalent metals in the layered inorganic mineral with trivalent metals. However, since introducing metal anions increases hydrophilicity, layered inorganic compounds in which at least a portion of the metal anions are modified with organic anions are preferred.
[0169] The layered inorganic mineral, in which at least a portion of the interlayer ions of the aforementioned layered inorganic mineral are modified with organic ions, can be obtained by using an organic cation modifier or an organic anion modifier.
[0170] The organic cation modifier is not particularly limited as long as it can be modified by organic ions as described above, and examples include quaternary alkylammonium salts, phosphonium salts, or imidazolium salts. These may be used individually or in combination of two or more. Among these, quaternary alkylammonium salts are preferred as the organic cation modifier.
[0171] The quaternary alkylammonium is not particularly limited, and examples include trimethylstearylammonium, dimethylstearylbenzylammonium, or oleylbis(2-hydroxyethyl)methylammonium.
[0172] The organic anion modifier is not particularly limited as long as it can be modified by organic ions as described above. Examples include sulfates, sulfonates, carboxylates, or phosphates having branched, unbranched, or cyclic alkyl (C1-C44) groups, branched, unbranched, or cyclic alkenyl (C1-C22) groups, branched, unbranched, or cyclic alkoxy (C8-C32) groups, branched, unbranched, or cyclic hydroxyalkyl (C2-C22) groups, an ethylene oxide skeleton, or a propylene oxide skeleton. These may be used individually or in combination of two or more. Among these, the organic anion modifier is preferably a carboxylic acid having an ethylene oxide skeleton.
[0173] The aforementioned shape-forming agent is preferably added in the oil phase preparation step in the process of manufacturing the resin particles. By modifying at least a portion of the interlayer ions of the layered inorganic mineral with organic ions, the material has appropriate hydrophobicity, so that the oil phase containing the resin particle material has non-Newtonian viscosity, and the resin particles can be deformed. In this case, the content of the deforming agent in the resin particle material is preferably 0.05% to 10% by mass, and more preferably 0.05% to 5% by mass, based on the total amount of the resin particle material.
[0174] Furthermore, there are no particular limitations on the layered inorganic mineral, and it can be appropriately selected depending on the purpose. Examples include montmorillonite, bentonite, hectorite, attapulgite, sepiolite, or mixtures thereof. Among these, layered inorganic minerals in which at least a portion of the interlayer ions are modified with organic ions are preferred because, when the resin particles are used in toner, they do not affect the toner characteristics, the viscosity can be easily adjusted, and the amount added can be small. Therefore, organically modified montmorillonite or organically modified bentonite is preferred.
[0175] Commercially available layered inorganic minerals in which at least a portion of the interlayer ions of the aforementioned layered inorganic mineral are modified with organic ions include, for example, quaternium-18 bentonite such as Bentone 3, Bentone 38, Bentone 38V (all manufactured by Rheox), Thixogel VP (manufactured by United Catalyst), Kraton 34, Kraton 40, Kraton XL (all manufactured by Southern Clay); stearalkonium bentonite such as Bentone 27 (manufactured by Rheox), Thixogel LG (manufactured by United Catalyst), Kraton AF, Kraton APA (all manufactured by Southern Clay); and quaternium-18 / benzalkonium bentonite such as Kraton HT, Kraton PS (both manufactured by Southern Clay). Among these, Kraton AF and Kraton APA are preferred.
[0176] Furthermore, as a layered inorganic mineral in which at least a portion of the interlayer ions of the layered inorganic mineral are modified with organic ions, it is more preferable to modify DHT-4A (registered trademark) (manufactured by Kyowa Chemical Industry Co., Ltd.) with an organic anion modifier represented by the following general formula (4). An example of an organic anion modifier represented by the following general formula (4) is Hythenol (registered trademark) 330T (manufactured by Daiichi Kogyo Seiyaku Co., Ltd.).
[0177] R1(OR2) n OSO3M...General formula (4) (In the general formula (4) above, R1 represents an alkyl group having 13 carbon atoms, R2 represents an alkylene group having 2 to 6 carbon atoms, n represents an integer of 2 to 10, and M represents a monovalent metal element.)
[0178] (Method for producing resin particles) The method for producing resin particles of the present invention includes: a) a step of preparing an oil phase in which at least an amorphous polyester resin and a crystalline resin are dissolved or dispersed in an organic solvent (hereinafter may be referred to as "oil phase preparation step"), b) a step of adding an aqueous medium to the oil phase to cause phase inversion from a water-in-oil dispersion to an oil-in-water dispersion (hereinafter may be referred to as "phase inversion emulsification step"), and c) a step of aggregating particles of the oil-in-water dispersion to obtain resin particles (hereinafter may be referred to as "aggregation step"), and optionally further includes other steps such as an aqueous phase preparation step, a desolvation step, a fusing step, a washing step, a drying step, a classification step, and an annealing step.
[0179] <a) Oil phase preparation step> The oil phase preparation step is a step of preparing an oil phase in which at least a resin is dissolved or dispersed in an organic solvent with stirring. The resin to be dissolved in the oil phase preparation step is as described above. The oil phase may further contain the colorant, the release agent, the crosslinking component and the like as needed.
[0180] The organic solvent is not particularly limited and may be appropriately selected according to the purpose, and an organic solvent having a boiling point of less than 150°C is preferred from the viewpoint of easy removal. The organic solvent with a boiling point below 150°C is not particularly limited and can be appropriately selected depending on the purpose. Examples include toluene, xylene, benzene, carbon tetrachloride, methylene chloride, 1,2-dichloroethane, 1,1,2-trichloroethane, trichloroethylene, chloroform, monochlorobenzene, dichloroethylidene, methyl acetate, ethyl acetate, methyl ethyl ketone, methyl isobutyl ketone, methanol, ethanol, or isopropyl alcohol. These may be used individually or in combination of two or more. Among these, ethyl acetate, toluene, xylene, benzene, methylene chloride, 1,2-dichloroethane, chloroform, or carbon tetrachloride are preferred as the organic solvent, with ethyl acetate being more preferred.
[0181] These organic solvents may be used individually or in combination of two or more.
[0182] When the resin to be dissolved or dispersed in an organic solvent is a resin having a polyester skeleton, it is preferable to use an ester-based solvent such as methyl acetate, ethyl acetate, or butyl acetate, or a ketone-based solvent such as methyl ethyl ketone or methyl isobutyl ketone, in order to achieve high solubility. Among these, methyl acetate, ethyl acetate, and methyl ethyl ketone are particularly preferred due to their high solvent removal properties.
[0183] There are no particular restrictions on the amount of the organic solvent used, and it can be appropriately selected depending on the purpose, but preferably 40 to 300 parts by mass, more preferably 60 to 140 parts by mass, and even more preferably 80 to 120 parts by mass per 100 parts by mass of the raw material for the resin particles.
[0184] There are no particular restrictions on the method for preparing the oil phase, and it can be appropriately selected depending on the purpose. For example, one method is to gradually add the materials for the oil phase to the organic solvent while stirring, and dissolve or disperse them. For the aforementioned dispersion, known methods can be used, such as dispersers like bead mills or disc mills.
[0185] There are no particular restrictions on the particle size of the dispersed crystalline resin in the oil phase, and it can be appropriately selected depending on the purpose, but it is preferably 20 nm to 500 nm, and more preferably 50 nm to 360 nm. In this specification, the dispersed particle size of the crystalline resin is the volume-average particle size.
[0186] The dispersed particle size of the crystalline resin can be measured, for example, using a nanotrack particle size distribution analyzer (UPA-EX150, Nikkiso Co., Ltd., dynamic light scattering method / laser Doppler method). The specific measurement method involves adjusting the dispersion of the crystalline resin to the measurement concentration range and then performing the measurement. Prior to this, a background measurement is performed using only the dispersion solvent of the dispersion. This method allows for measurements from several tens of nanometers to several micrometers.
[0187] <Aqueous phase (aqueous medium) production process> The aforementioned aqueous phase preparation step is a step of preparing an aqueous phase (aqueous medium). The aqueous medium is not particularly limited and can be appropriately selected depending on the purpose. Examples include water, a solvent miscible with water, or a mixture thereof. These may be used individually or in combination of two or more. Among these, water is preferred.
[0188] The solvent that can be miscible with water is not particularly limited and can be appropriately selected depending on the purpose. Examples include alcohols, dimethylformamide, tetrahydrofuran, ethyl acetate, cellosolves, or lower ketones. The aforementioned alcohol is not particularly limited and can be appropriately selected depending on the purpose. Examples include methanol, isopropanol, or ethylene glycol. The aforementioned lower ketones are not particularly limited and can be appropriately selected depending on the purpose. Examples include acetone or methyl ethyl ketone. Sodium dodecyl sulfate may also be added to the aqueous phase.
[0189] <b)Phase inversion emulsification step> The phase inversion emulsification step is a step of adding an aqueous medium to the oil phase to invert the phase from a water-in-oil dispersion to an oil-in-water dispersion. Thereby, a fine particle dispersion (oil droplets) is obtained. Further, when the oil phase contains the non-linear reactive precursor, an amorphous polyester resin may be produced by subjecting the curing agent and the non-linear reactive precursor to an elongation reaction and / or a crosslinking reaction in the phase inversion emulsification step. The amorphous polyester resin is as described in the section of <<Amorphous Polyester Resin>> for the above (resin particles, toner resin, and coating resin particles).
[0190] When the amorphous polyester resin is produced in the phase inversion emulsification step, specifically, the amorphous polyester resin can be produced by, for example, any one of the following methods (1) to (3). (1) A method of emulsifying or dispersing an oil phase containing the non-linear reactive precursor and the curing agent in the aqueous medium, and subjecting the curing agent and the non-linear reactive precursor to an elongation reaction and / or a crosslinking reaction in the aqueous medium to produce the amorphous polyester resin. (2) A method of emulsifying or dispersing an oil phase containing the non-linear reactive precursor in an aqueous medium to which the curing agent has been added in advance, and subjecting the curing agent and the non-linear reactive precursor to an elongation reaction and / or a crosslinking reaction in the aqueous medium to produce the amorphous polyester resin. (3) A method of emulsifying or dispersing an oil phase containing the non-linear reactive precursor in an aqueous medium, then adding the curing agent to the aqueous medium, and subjecting the curing agent and the non-linear reactive precursor to an elongation reaction and / or a crosslinking reaction from the particle interface in the aqueous medium to produce the amorphous polyester resin.
[0191] Furthermore, when the curing agent and the nonlinear reactive precursor are subjected to an extension reaction and / or crosslinking reaction from the resin particle interface, the amorphous polyester resin is preferentially formed on the surface of the resulting resin particles, and a concentration gradient of the amorphous polyester resin can be provided within the resin particles.
[0192] There are no particular restrictions on the reaction conditions (reaction time, reaction temperature) for producing the amorphous polyester resin, and they can be appropriately selected depending on the combination of the curing agent and the nonlinear reactive precursor. There are no particular restrictions on the reaction time, and it can be appropriately selected depending on the purpose, but it is preferably between 10 minutes and 40 hours, and more preferably between 2 hours and 24 hours. The reaction temperature is not particularly limited and can be appropriately selected depending on the purpose, but it is preferably 0°C to 150°C, and more preferably 40°C to 98°C.
[0193] There are no particular limitations on the method for phase-inversion emulsification of the dispersion containing the nonlinear reactive precursor in the aqueous medium, and a suitable method can be selected depending on the purpose. For example, one method involves neutralizing the oil phase with a base, then adding the aqueous phase to it, and obtaining a fine particle dispersion by phase-inversion emulsification, which converts the water-in-oil dispersion to an oil-in-water dispersion.
[0194] There are no particular restrictions on the base used to neutralize the oil phase, and it can be appropriately selected depending on the purpose. Examples include sodium hydroxide, potassium hydroxide, or aqueous ammonia.
[0195] There are no particular restrictions on the amount of the aqueous medium used when emulsifying the oil phase containing the resin particle material, and it can be appropriately selected according to the purpose. Preferably, the amount is 50 parts by mass or more and 2,000 parts by mass or less, and more preferably 100 parts by mass or more and 1,000 parts by mass or less, per 100 parts by mass of the resin particle material. If the amount of the aqueous medium used is 50 parts by mass or more per 100 parts by mass of the resin particle material, it is possible to prevent the dispersion state of the resin particle material from deteriorating and to suppress the inability to obtain resin particles of a predetermined particle size. Furthermore, if the amount of the aqueous medium used is 2,000 parts by mass or less per 100 parts by mass of the resin particle material, it is possible to suppress the increase in production costs.
[0196] When inverting the oil phase containing the aforementioned resin particle material, it is preferable to use a dispersant from the viewpoint of stabilizing the dispersion, such as oil droplets, to achieve the desired shape and sharpen the particle size distribution. There are no particular restrictions on the dispersant, and it can be appropriately selected depending on the purpose. Examples include surfactants, poorly water-soluble inorganic compound dispersants, or polymer-based protective colloids. These may be used individually or in combination of two or more. Among these, surfactants are preferred as the dispersant.
[0197] The surfactant is not particularly limited and can be appropriately selected depending on the purpose. Examples include anionic surfactants, cationic surfactants, nonionic surfactants, or amphoteric surfactants.
[0198] The anionic surfactant is not particularly limited and can be appropriately selected depending on the purpose. Examples include alkylbenzene sulfonates, α-olefin sulfonates, or phosphate esters. Among these, the anionic surfactant having a fluoroalkyl group is preferred.
[0199] A catalyst can be used in the extension reaction and / or crosslinking reaction when producing the amorphous polyester resin. The catalyst is not particularly limited and can be appropriately selected depending on the purpose. Examples include dibutylsulfurate and dioctylsulfurate.
[0200] The aforementioned phase inversion emulsification can be carried out using a stirring blade. The aforementioned stirring blades are not particularly limited and can be appropriately selected depending on the viscosity of the solution. Examples include anchor blades, turbine blades, Faudler blades, full-zone blades, maxblend blades, or crescent blades.
[0201] When using the aforementioned stirring blade, there are no particular restrictions on the peripheral speed, and it can be appropriately selected depending on the purpose, but 0.4 m / sec to 2.0 m / sec is preferred, and 0.7 m / sec to 1.5 m / sec is more preferred.
[0202] There are no particular restrictions on the volume-average particle size of the dispersion (oil droplets) in the fine particle dispersion, and it can be appropriately selected depending on the purpose, but 50 nm to 2,000 nm is preferred, and 50 nm to 500 nm is more preferred.
[0203] <Solvent removal process> The solvent removal step is a step of removing the organic solvent from the fine particle dispersion obtained in the phase inversion emulsification step to obtain a slurry containing resin matrix particles.
[0204] There are no particular limitations on the method for removing the organic solvent from the fine particle dispersion, and a suitable method can be selected depending on the purpose. Examples include gradually raising the temperature of the entire reaction system to evaporate the organic solvent in the fine particle dispersion (oil droplets); spraying the fine particle dispersion into a dry atmosphere to remove the organic solvent in the fine particle dispersion (oil droplets); and reducing the pressure of the fine particle dispersion to evaporate and remove the organic solvent. These may be used individually or in combination of two or more types.
[0205] There are no particular restrictions on the drying atmosphere in which the fine particle dispersion is sprayed, and it can be appropriately selected depending on the purpose. Examples include heated air, nitrogen, carbon dioxide, combustion gas, etc. In general, various gas streams heated to a temperature above the boiling point of the highest boiling point solvent used are used.
[0206] The solvent removal process can be carried out using equipment, such as a spray dryer, belt dryer, or rotary kiln, and the desired quality can be obtained in a short processing time.
[0207] <Process for preparing resin particles that do not contain plant-derived ingredients> Except for using a) an oil phase preparation step and b) a phase inversion emulsification step, the same method as described above can be used to desolvate the oil phase and obtain resin particles to be used only for the shell.
[0208] <Preparation process of resin particles for shells> A step in preparing resin particles for the shell of the resin particles of the present invention, comprising mixing [slurry A] containing resin matrix particles containing plant-derived components, which are produced in the <solvent removal step> of the b) phase inversion emulsification step, with [slurry B] containing resin matrix particles that do not contain plant-derived components, which are produced in the same manner as the <solvent removal step> of the b) phase inversion emulsification step.
[0209] The resin particles for the shell obtained by mixing the [slurry A] and the [slurry B] can further form a core-shell structure, the core of the core-shell structure may mainly contain [slurry A], and the shell of the core-shell structure may mainly contain [slurry B]. Since it is preferable that the surface of the resin particles of the present invention contains few or no plant-derived components that worsen filming properties, in the core-shell structure further formed on the resin particles for the shell, it is preferable that the shell mainly contains [slurry B] and the core mainly contains [slurry A].
[0210] When the core of the core-shell structure, which is formed by the aforementioned shell resin particles, mainly contains [Slurry A], the shell layer of the resin particles of the present invention produced from the shell resin particles of this configuration can have a structure having domains mainly containing "a resin containing a plant-derived component", and the resin contained in the outermost surface portion of the resin particles of the present invention can be configured to mainly contain "a resin containing no plant-derived component". By using a resin with such a configuration as the shell resin, resin particles having excellent heat-resistant storage stability can be produced.
[0211] <c) Aggregation step> The aggregation step is a step of aggregating the particles of the oil-in-water dispersion to obtain aggregated particles. The method for aggregating the oil droplets or the base particles is not particularly limited, and can be appropriately selected from known methods according to the purpose, and examples thereof include a method of adding an aggregating agent, a method of performing pH adjustment, and the like.
[0212] There are no particular restrictions on the aforementioned flocculant, and it can be appropriately selected depending on the purpose. For example, aluminum chloride, zinc sulfate, magnesium sulfate, aluminum sulfate, potassium aluminum sulfate, sodium chloride, sodium bromide, sodium iodide, sodium fluoride, sodium acetate, sodium acetoacetate, lithium chloride, lithium bromide, lithium iodide, lithium fluoride, lithium acetate, lithium acetoacetate, potassium chloride, potassium bromide, potassium iodide, potassium fluoride, potassium acetoacetate, magnesium bromide, magnesium chloride, magnesium iodide, fluoride Examples include magnesium, magnesium acetate, magnesium acetoacetate, calcium chloride, calcium bromide, barium bromide, barium chloride, barium iodide, barium fluoride, barium acetate, barium acetoacetate, strontium bromide, strontium chloride, strontium iodide, strontium fluoride, strontium acetate, strontium acetoacetate, zinc bromide, zinc chloride, zinc iodide, zinc fluoride, zinc acetate, zinc acetoacetate, copper bromide, copper chloride, copper iodide, copper fluoride, copper acetate, copper acetoacetate, iron bromide, iron chloride, iron iodide, iron fluoride, iron acetate, or iron acetoacetate. These may be used individually or in combination of two or more. Among these, divalent metal salts are preferred as the flocculant, and trivalent metal salts are more preferred. By using a metal salt with a valency of two or more, a three-dimensional structure can be formed by metal crosslinking with the carboxyl groups contained in the amorphous polyester resin, thereby increasing the strength of the resin particles and improving filming resistance.
[0213] When adding the aforementioned flocculant, it may be added as is, but it is preferable to use an aqueous solution of the flocculant to avoid localized high concentrations. Furthermore, it is preferable to add the flocculant gradually while observing the particle size of the resin particles.
[0214] There are no particular restrictions on the temperature of the reaction system in which the agglomeration process is carried out (temperature of the dispersion during agglomeration), and it can be appropriately selected according to the purpose. However, it is preferably near the glass transition temperature (Tg) of the resin used, and more preferably near the glass transition temperature (Tg) of the amorphous polyester resin. If the temperature of the reaction system is too low, agglomeration will not proceed well, which may result in poor efficiency. If the temperature of the reaction system is too high, the agglomeration rate will be too fast, which may lead to the generation of coarse particles and a deterioration of the particle size distribution.
[0215] The aggregation process stops after the aggregated particles reach the desired particle size. There are no particular restrictions on the method for stopping the aggregation, and it can be appropriately selected depending on the purpose. For example, methods such as adding a salt or chelating agent with a lower ionic charge than the aggregation salt; adjusting the pH; lowering the temperature of the reaction system (dispersion) during aggregation; or diluting the concentration of the reaction system (dispersion) during aggregation by adding a large amount of aqueous medium can be used. These may be used individually or in combination of two or more types.
[0216] There are no particular restrictions on the volume-average particle size of the aggregated particles, and they can be appropriately selected depending on the purpose, but 3.0 μm to 6.0 μm is preferred, and 4.0 μm to 5.0 μm is more preferred.
[0217] In the aggregation step, a mold release agent may be added, and the crystalline resin may be added for low-temperature fixation. As the release agent, the above-mentioned release agent (wax) can be used. When adding the mold release agent or the crystalline resin in the aforementioned aggregation process, a dispersion of the mold release agent in an aqueous medium, or similarly a dispersion of the crystalline polyester resin, can be prepared and mixed with the fine particle dispersion (oil droplets) before aggregation, thereby obtaining aggregated particles in which the mold release agent or crystalline resin is uniformly dispersed.
[0218] There are no particular restrictions on the particle size of the release agent dispersed in the dispersion, and it can be appropriately selected depending on the purpose, but it is preferably 50 nm to 600 nm, and more preferably 50 nm to 300 nm. In this specification, the particle size of the release agent dispersed in the dispersion is the volume-average particle size.
[0219] The dispersed particle size of the aforementioned release agent can be measured, for example, using a NanoTrac particle size distribution analyzer (UPA-EX150, Nikkiso Co., Ltd., dynamic light scattering method / laser Doppler method). The specific measurement method involves adjusting the dispersion containing the release agent to the measurement concentration range and then performing the measurement. Prior to this, a background measurement is performed using only the dispersion solvent of the dispersion. This method allows for measurements from several tens of nanometers to several micrometers.
[0220] Furthermore, in order to form a shell layer on the resin particles, a dispersion of shell resin may be added in the aggregation step. By forming a shell layer on the resin particles, the crystalline resin and release agent that would otherwise worsen the filming properties can be encapsulated, thereby improving filming resistance.
[0221] There are no particular limitations on the method for forming the shell layer, and it can be appropriately selected depending on the purpose. For example, one method is to produce aggregated particles by the method described above, and then add the shell resin to the aggregated particles that have reached a desired particle size. Furthermore, if the method for producing the resin particles includes the solvent removal step, after obtaining a slurry of aggregated particles of the matrix particles obtained in the solvent removal step, the slurry of the shell resin may be added to obtain the aggregated slurry.
[0222] <Fusing process> The fusion step is a step of fusing the aggregated particles or the slurry containing the aggregated particles to reduce irregularities and obtain spherical resin particles. Furthermore, if resin is added in the aggregation step to form a shell layer on the resin particles, the fusion step can form a shell layer on the surface of the aggregated particles.
[0223] There are no particular limitations on the method for fusing the aggregated particles, and a suitable method can be selected depending on the purpose. For example, a method of heating the dispersion of the aggregated particles while stirring can be used.
[0224] There are no particular restrictions on the heating temperature, and it can be appropriately selected depending on the purpose, but it is preferably between Tg and Tg+20°C of the amorphous polyester resin, and more preferably between Tg and Tg+10°C. When the heating temperature is below Tg+20°C of the amorphous polyester resin, the amorphous polyester resin and the crystalline resin become appropriately compatible, improving heat resistance and storage properties.
[0225] There are no particular restrictions on the average circularity of the resin particles, and they can be appropriately selected depending on the purpose. However, a higher average circularity of the resin particles is preferable, as it allows them to rotate more smoothly in the developing nip when used as toner, thus enabling more resin particles to transfer to the electrostatic latent image carrier. In this respect, a circularity of 0.95 or higher is preferable, and 0.96 or higher is more preferable.
[0226] -Measurement of average particle diameter and average circularity- In this embodiment, the average particle diameter and average circularity can be measured, for example, using a flow-type particle image analyzer (FPIA-3000, manufactured by Sysmex Corporation). The specific measurement method involves adding 0.1 mL to 0.5 mL of a surfactant, preferably alkylbenzene sulfonate, as a dispersant to 100 mL to 150 mL of water from which impurities have been removed beforehand, and then adding approximately 0.1 g to 0.5 g of the sample to be measured. The suspension in which the sample is dispersed is subjected to dispersion treatment in an ultrasonic disperser for approximately 1 to 3 minutes, and the dispersion concentration is set to 3,000 particles / μL to 10,000 particles / μL. The average particle size, average circularity, and standard deviation (SD) of circularity are then measured using the aforementioned apparatus. However, the particle diameter shall be the equivalent diameter of a circle, the average particle diameter shall be determined by the equivalent diameter of a circle (based on the number of particles), and the analysis conditions for the flow-type particle image analyzer shall be as follows. [Analysis conditions] Particle diameter limitation: 0.5 μm ≤ equivalent circle diameter (number basis) ≤ 200.0 μm Particle shape limitation: 0.93 < circularity ≤ 1.00 Further, the definition of the average circularity in the present embodiment is as follows. (Average circularity) = (Perimeter of a circle having the same area as the projected area of the particle) / (Perimeter of the projected image of the particle)
[0227] <Washing step> The washing step is a step of washing the resin particles obtained in the aggregation step or the fusing step. Since the dispersion liquid of resin particles obtained by the above-described method may contain auxiliary materials such as a flocculant in addition to the resin particles, washing is preferably performed to extract only the resin particles from the dispersion liquid of resin particles.
[0228] The method for washing the resin particles is not particularly limited and may be appropriately selected according to the purpose, and examples thereof include a centrifugation method, a reduced-pressure filtration method, and a filter press method. A cake body of the resin particles can be obtained by any of the washing methods. When sufficient washing cannot be performed in a single operation, the obtained cake body may be re-dispersed in an aqueous solvent to form a slurry, and the step of extracting the resin particles by at least any one of the above washing methods may be repeated. When washing is performed by the reduced-pressure filtration method or the filter press method, a method may be adopted in which an aqueous solvent is passed through the cake body to wash away the auxiliary materials entrapped by the resin particles.
[0229] The aqueous solvent used in the washing step is not particularly limited and may be appropriately selected according to the purpose, and examples thereof include water, or a mixed solvent of water and an alcohol. Examples of the alcohol include methanol or ethanol. Among these, the aqueous solvent is preferably water from the viewpoint of environmental load such as cost and wastewater treatment.
[0230] <Drying step> The drying step is a step of washing the resin particles obtained in the washing step. Since the resin particles washed in the washing step contain a large amount of the aqueous medium, drying them in the drying step removes the aqueous medium, allowing only the resin particles to be obtained.
[0231] There are no particular restrictions on the drying method, and it can be appropriately selected according to the purpose. Examples include using a spray dryer, vacuum freeze dryer, reduced pressure dryer, stationary shelf dryer, mobile shelf dryer, fluidized bed dryer, rotary dryer, or agitated dryer.
[0232] There are no particular restrictions on the final moisture content of the dried resin particles, and it can be appropriately selected depending on the purpose, but it is preferable that the moisture content is less than 1% by mass.
[0233] The resin particles dried in the aforementioned drying process are soft and aggregated. If this causes problems during use, they may be crushed to break up the aggregates. There are no particular restrictions on the method of crushing, and it can be appropriately selected depending on the purpose. Examples include using a jet mill, Henschel mixer, super mixer, coffee mill, Auster blender, or food processor.
[0234] <Classification process> The classification process is a process of classifying the resin particles obtained in the washing process or the drying process. There are no particular restrictions on the classification method, and it can be appropriately selected depending on the purpose. Examples include methods that remove fine particles in a liquid using a cyclone, decanter, centrifugation, etc., or methods that perform known classification operations after drying.
[0235] <Annealing Process> The annealing step is performed after the drying step when a crystalline resin is added, and is a step that separates the crystalline resin from the amorphous polyester resin.
[0236] There are no particular restrictions on the method of performing the annealing treatment, and it can be appropriately selected depending on the purpose, but examples include storing the crystalline resin at a temperature near its glass transition temperature (Tg) for 10 hours or more.
[0237] In the aforementioned fusion process, if the resin used is heated to a temperature near the glass transition temperature (Tg) of the resin, the crystalline resin and the amorphous polyester resin may become miscible, making it impossible to achieve both heat resistance and low-temperature fixation. However, performing the annealing treatment promotes phase separation between the crystalline resin and the amorphous resin, eliminating the miscible state, which is advantageous and can contribute to improved fixation.
[0238] (toner) The toner according to this embodiment includes the resin particles described above. That is, the toner of this embodiment includes resin particles having a core-shell structure having a core containing the first resin described above and a shell containing the second resin described above.
[0239] The toner of the present invention preferably further contains an external additive, and may further contain other components as needed. In the toner of the present invention, the resin particles of the present invention are resin particles for toner and can become toner matrix particles of the present invention.
[0240] There are no particular restrictions on the content of the toner resin particles in the toner, and it can be appropriately selected depending on the purpose. The toner may also be the toner resin particles themselves.
[0241] -External additives- There are no particular restrictions on the external additives, and they can be appropriately selected depending on the purpose. Examples include inorganic fine particles, oxide fine particles, fatty acid metal salts, or hydrophobized versions thereof. These may be used individually or in combination of two or more.
[0242] There are no particular restrictions on the average particle size of the primary particles of the inorganic fine particles, and it can be appropriately selected depending on the purpose, but it is preferably 100 nm or less, more preferably 1 nm to 100 nm, even more preferably 3 nm to 70 nm, and particularly preferably 5 nm to 70 nm. If the average particle size of the primary particles of the inorganic fine particles is 1 nm or more, it is possible to prevent the inorganic fine particles from becoming embedded in the toner and not being able to effectively perform their function, and if it is 100 nm or less, it is possible to suppress uneven scratching of the photoreceptor surface.
[0243] Furthermore, it is preferable that the inorganic fine particles include at least one type of inorganic fine particles having an average primary particle size of 20 nm or less, and at least one type of inorganic fine particles having an average primary particle size of 30 nm or more.
[0244] There are no particular restrictions on the specific surface area of the inorganic fine particles obtained by the BET method, and it can be appropriately selected according to the purpose, but 20m 2 / g or more 500m 2 It is preferable that the value be less than or equal to / g.
[0245] The inorganic fine particles are not particularly limited and can be appropriately selected depending on the purpose. Examples include silica, alumina, titanium oxide, barium titanate, magnesium titanate, calcium titanate, strontium titanate, iron oxide, copper oxide, zinc oxide, tin oxide, silica sand, clay, mica, wollastonite, diatomaceous earth, chromium oxide, cerium oxide, red iron oxide, antimony trioxide, magnesium oxide, zirconium oxide, barium sulfate, barium carbonate, calcium carbonate, silicon carbide, or silicon nitride. These may be used individually or in combination of two or more. Among these, silica or titanium dioxide are preferred.
[0246] The oxide fine particles are not particularly limited and can be appropriately selected depending on the purpose. Examples include titania, alumina, tin oxide, or antimony oxide.
[0247] Examples of the fatty acid metal salt include zinc stearate and aluminum stearate.
[0248] Among these, the external additive is preferably hydrophobic-treated fine particles of silica, titania, titanium oxide, or alumina.
[0249] Examples of the silica fine particles include R972, R974, RX200, RY200, R202, R805, and R812 (all manufactured by Nippon Aerosil Co., Ltd.).
[0250] Examples of the titania fine particles include P-25 (manufactured by Nippon Aerosil Co., Ltd.), STT-30, STT-65C-S (all manufactured by Titan Kogyo, Ltd.), TAF-140 (manufactured by Fuji Titanium Industry Co., Ltd.), MT-150W, MT-500B, MT-600B, and MT-150A (all manufactured by Tayca Corporation).
[0251] Examples of the hydrophobic-treated titanium oxide fine particles include T-805 (manufactured by Nippon Aerosil Co., Ltd.), STT-30A, STT-65S-S (all manufactured by Titan Kogyo, Ltd.), TAF-500T, TAF-1500T (all manufactured by Fuji Titanium Industry Co., Ltd.), MT-100S, MT-100T (all manufactured by Tayca Corporation), and IT-S (manufactured by Ishihara Sangyo Kaisha, Ltd.).
[0252] The hydrophobic-treated oxide fine particles, hydrophobic-treated silica fine particles, hydrophobic-treated titania fine particles, or hydrophobic-treated alumina fine particles can be obtained, for example, by treating hydrophilic fine particles with a silane coupling agent such as methyltrimethoxysilane, methyltriethoxysilane, or octyltrimethoxysilane. Further, silicone oil-treated oxide fine particles and inorganic fine particles, which are obtained by treating inorganic fine particles with silicone oil under heating if necessary, are also suitable. In addition, the external additive may be subjected to surface treatment using the <<fluidity improver>> for the (resin particles, toner resins, and coating resin particles).
[0253] The silicone oil is not particularly limited and can be appropriately selected depending on the purpose. Examples include dimethyl silicone oil, methylphenyl silicone oil, chlorophenyl silicone oil, methyl hydrogen silicone oil, alkyl-modified silicone oil, fluorine-modified silicone oil, polyether-modified silicone oil, alcohol-modified silicone oil, amino-modified silicone oil, epoxy-modified silicone oil, epoxy-polyether-modified silicone oil, phenol-modified silicone oil, carboxyl-modified silicone oil, mercapto-modified silicone oil, methacrylic-modified silicone oil, or α-methylstyrene-modified silicone oil.
[0254] There are no particular restrictions on the content of the external additive, and it can be appropriately selected depending on the purpose, but it is preferably 0.01% to 5% by mass, and more preferably 1% to 3% by mass, based on 100% by mass of the toner.
[0255] There are no particular restrictions on the method for manufacturing the toner, and any known method can be appropriately selected; however, it is preferable that the toner be manufactured by the method for manufacturing toner of the present invention, which will be described later.
[0256] (Toner manufacturing method) The toner manufacturing method of the present invention includes a mixing step of mixing resin particles for the toner of the present invention with an external additive, and further includes other steps as necessary.
[0257] The resin particles for the toner are as described above, and the external additive is also as described above; details are omitted.
[0258] <Mixing process> The mixing step involves mixing the toner resin particles, which serve as the toner matrix particles, with the external additive. Applying a mechanical impact force at this stage is preferable because it can suppress the detachment of the external additive particles from the surface of the toner matrix particles.
[0259] There are no particular limitations on the method of applying the mechanical impact force, and it can be appropriately selected depending on the purpose. Examples include a method of applying impact force to the mixture of the toner resin particles and the external additive using a blade that rotates at high speed; and a method of introducing the mixture of the toner resin particles and the external additive into a high-speed airflow, accelerating it, and causing the particles to collide with each other or with a suitable impact plate.
[0260] There are no particular restrictions on the devices used in the method of applying the aforementioned mechanical impact force, and they can be appropriately selected according to the purpose. Examples include an Ongmill (manufactured by Hosokawa Micron Corporation), a modified I-type mill (manufactured by Nippon Pneumatic Mfg. Co., Ltd.) with reduced grinding air pressure, a hybridization system (manufactured by Nara Machinery Works Co., Ltd.), a cryptron system (manufactured by Kawasaki Heavy Industries, Ltd.), and an automatic mortar and pestle.
[0261] (Developer) The developer of the present invention contains at least the toner of the present invention, and further contains other components that are appropriately selected, such as a carrier, as needed. The toner contained in the developer of the present invention contains the toner resin particles of the present invention, and therefore the developer is highly environmentally friendly, highly carbon neutral, and has excellent heat resistance for storage. For this reason, the developer has excellent transferability, electrostatic properties, etc., and can stably form high-quality images.
[0262] The developer may be a one-component developer or a two-component developer, but when used in high-speed printers and the like to accommodate the recent increase in information processing speed, a two-component developer is preferred because it extends the lifespan.
[0263] When the developer is used as a single-component developer, even when the toner is balanced, there is little variation in the particle size of the toner, resulting in less toner filming onto the developing roller and less toner fusion onto components such as blades that thin the toner layer. This allows for good and stable development and image quality even during long-term agitation in the developing apparatus.
[0264] When the aforementioned developer is used as a two-component developer, even with long-term toner balance, there is little variation in toner particle size, and good and stable developability and images can be obtained even with long-term agitation in the developing device.
[0265] <Career> There are no particular restrictions on the carrier, and it can be appropriately selected according to the purpose, but one having a core material and a resin layer covering the core material is preferred.
[0266] <<Core material>> There are no particular restrictions on the core material, and it can be appropriately selected according to the purpose. For example, manganese-strontium materials with a magnetization of 50 emu / g to 90 emu / g, or manganese-magnesium materials with a magnetization of 50 emu / g to 90 emu / g are examples. Furthermore, in order to ensure image density, it is preferable to use highly magnetized materials such as iron powder of 100 emu / g or more, or magnetite with a magnetization of 75 emu / g to 120 emu / g. In addition, it is preferable to use low magnetized materials such as copper-zinc materials with a magnetization of 30 emu / g to 80 emu / g, as this can mitigate the impact of the developer in a condensed state on the photoreceptor and is advantageous for improving image quality. These can be used individually or in combination of two or more.
[0267] There are no particular restrictions on the volume-average particle diameter of the core material, and it can be appropriately selected according to the purpose, but it is preferably 10 μm to 150 μm, and more preferably 40 μm to 100 μm. When the volume-average particle diameter of the core material is 10 μm or more, it is possible to prevent a large amount of fine powder from accumulating in the carrier, and to suppress the decrease in magnetization per particle and the resulting scattering of carriers. Furthermore, when the volume-average particle diameter of the core material is 150 μm or less, it is possible to prevent a decrease in specific surface area and to suppress the scattering of toner, and in full-color printing with many solid areas, it is possible to suppress the deterioration of reproduction of solid areas in particular.
[0268] When the toner is used in a two-component developer, it may be used in combination with the carrier. There are no particular restrictions on the amount of the carrier in the two-component developer, and it can be appropriately selected depending on the purpose, but it is preferably 90 parts by mass or more and 98 parts by mass or less, and more preferably 93 parts by mass or more and 97 parts by mass or less, per 100 parts by mass of the two-component developer.
[0269] The developer can be suitably used for image formation by various known electrophotographic methods, including magnetic one-component development methods, non-magnetic one-component development methods, or two-component development methods.
[0270] (Toner storage unit) The toner storage unit of the present invention is a unit having the function of storing toner, in which toner is stored. The toner contained in the toner storage unit is the toner of the present invention. Therefore, the toner storage unit of the present invention is highly environmentally friendly. Furthermore, since image formation is performed using the toner of the present invention when the toner storage unit is mounted in the image forming apparatus of the present invention, it exhibits high carbon neutrality and excellent heat resistance for storage.
[0271] The configuration of the toner storage unit is not particularly limited as long as it can accommodate the toner, and can be appropriately selected according to the purpose. Examples include a toner storage container, a developer, or a process cartridge.
[0272] <Toner container> The toner container mentioned above refers to a container that contains the toner. The toner storage container is not particularly limited and can be appropriately selected from known types, for example, one having a container body and a cap.
[0273] The size of the container body is not particularly limited and can be changed as appropriate.
[0274] The shape of the container body is not particularly limited and can be changed as appropriate, but it is preferably cylindrical.
[0275] The structure of the container body is not particularly limited and can be modified as appropriate, but a structure is preferred in which spiral-shaped irregularities are formed on the inner surface, and the toner contents can be moved to the discharge port side by rotating the container, and in which part or all of the spiral-shaped irregularities have a bellows function.
[0276] The material of the container body is not particularly limited and can be changed as appropriate, but it is preferable that it has good dimensional accuracy. Examples include resin materials such as polyester resin, polyethylene resin, polypropylene resin, polystyrene resin, polyvinyl chloride resin, polyacrylic acid, polycarbonate resin, ABS resin, or polyacetal resin. These may be used individually or in combination of two or more.
[0277] The toner storage container is easy to store and transport, and has excellent handling properties, so it can be detachably attached to a process cartridge or image forming apparatus and used for replenishing the toner.
[0278] <developer> The term "developer" refers to a device that houses the toner and has a developing mechanism. The developing means is not particularly limited and can be appropriately selected according to the purpose. For example, it may include at least a toner storage container and a toner carrier that carries and transports the toner stored in the toner storage container. Furthermore, the developing means may include regulating members or the like to control the thickness of the toner it carries.
[0279] <Processing Cartridge> The process cartridge refers to a device that integrates at least an electrostatic latent image carrier and a developing means, contains the toner, and is detachable from the image forming apparatus. The process cartridge may further have at least one selected from a charging means, an exposure means, a cleaning means, and a static elimination means, as needed.
[0280] An example of the process cartridge is one which is molded to be detachable from various image forming apparatuses and has at least an electrostatic latent image carrier that carries an electrostatic latent image, and a developing means that develops the electrostatic latent image carried on the electrostatic latent image carrier with the toner to form a toner image, and may have other means as needed. [Examples]
[0281] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. In the following, "parts" refers to mass unless otherwise specified. Furthermore, various tests and evaluations will be carried out according to the methods described below.
[0282] The synthesis of amorphous polyester resin is described below. When synthesizing the amorphous polyester resin, resins containing plant-derived alcohol monomer units and resins containing non-plant-derived monomer units were added in the proportions shown in Table 1.
[0283] <Synthesis of amorphous polyester resin B-1> In a four-necked flask equipped with a nitrogen inlet tube, dehydration tube, stirrer, and thermocouple, plant-derived propylene glycol (Dupont), bisphenol A propylene oxide 2-mol adduct, terephthalic acid, and plant-derived succinic acid (Bioamber) were added, with the molar ratio of plant-derived propylene glycol to bisphenol A ethylene oxide 2-mol adduct being 30 / 70, and terephthalic acid and succinic acid being added. The terephthalic acid and succinic acid were charged in a molar ratio (terephthalic acid / succinic acid) of 86 / 14, and the molar ratio of hydroxyl groups to carboxyl groups (OH / COOH) was 1.3. This mixture was reacted with titanium tetraisopropoxide (500 ppm relative to the resin components) at atmospheric pressure and 230°C for 8 hours, followed by a further reaction under reduced pressure of 10 mmHg to 15 mmHg for 4 hours. Finally, trimellitic anhydride was added to the reaction vessel in a ratio of 1 mol% relative to the total resin components, and the mixture was reacted at 180°C and atmospheric pressure for 3 hours to obtain [amorphous polyester resin B-1]. The weight-average molecular weight of the obtained [amorphous polyester resin B-1] was 6000.
[0284] <Synthesis of amorphous polyester resin B-2> In a four-necked flask equipped with a nitrogen inlet tube, dehydration tube, stirrer, and thermocouple, plant-derived propylene glycol, bisphenol A propylene oxide 2-mol adduct, terephthalic acid, and plant-derived succinic acid were added, with the molar ratio of plant-derived propylene glycol to bisphenol A ethylene oxide 2-mol adduct being 20 / 80, and the molar ratio of terephthalic acid to succinic acid being 20 / 80. The taric acid / succinic acid mixture was 86 / 14, and the molar ratio of hydroxyl groups to carboxyl groups (OH / COOH) was set to 1.3. This mixture was then reacted with titanium tetraisopropoxide (500 ppm relative to the resin components) at atmospheric pressure and 230°C for 8 hours. After further reaction under reduced pressure of 10 mmHg to 15 mmHg for 4 hours, trimellitic anhydride was added to the reaction vessel at a concentration of 1 mol% relative to the total resin components, and the mixture was reacted at 180°C and atmospheric pressure for 3 hours to obtain [amorphous polyester resin B-2]. The weight-average molecular weight of the obtained [amorphous polyester resin B-2] was 5500.
[0285] <Synthesis of amorphous polyester resin B-3> In a four-necked flask equipped with a nitrogen inlet tube, dehydration tube, stirrer, and thermocouple, plant-derived propylene glycol, bisphenol A propylene oxide 2-mol adduct, terephthalic acid, and plant-derived succinic acid were added, with the molar ratio of plant-derived propylene glycol to bisphenol A ethylene oxide 2-mol adduct being 4 / 96, and the molar ratio of terephthalic acid to succinic acid being 4 / 96. The mixture was prepared with a ratio of 86 / 14 (hydroxyl acid / succinic acid) and a molar ratio of OH / COOH (hydroxyl group to carboxyl group) of 1.3. It was reacted with titanium tetraisopropoxide (500 ppm relative to the resin component) at atmospheric pressure and 230°C for 8 hours, and then reacted again for 4 hours under reduced pressure of 10 mmHg to 15 mmHg. Finally, trimellitic anhydride was added to the reaction vessel at a concentration of 1 mol% relative to the total resin component, and the mixture was reacted at 180°C and atmospheric pressure for 3 hours to obtain [amorphous polyester resin B-3]. The weight-average molecular weight of the obtained [amorphous polyester resin B-3] was 6500.
[0286] <Synthesis of amorphous polyester resin B-4> In a four-necked flask equipped with a nitrogen inlet tube, dehydration tube, stirrer, and thermocouple, plant-derived propylene glycol, bisphenol A propylene oxide 2-mol adduct, terephthalic acid, and plant-derived succinic acid were added, with the molar ratio of plant-derived propylene glycol to bisphenol A ethylene oxide 2-mol adduct being 40 / 60, and the molar ratio of terephthalic acid to succinic acid being 40 / 60. The taric acid / succinic acid mixture was 86 / 14, and the molar ratio of hydroxyl groups to carboxyl groups (OH / COOH) was set to 1.3. This mixture was then reacted with titanium tetraisopropoxide (500 ppm relative to the resin components) at atmospheric pressure and 230°C for 8 hours. After further reaction under reduced pressure of 10 mmHg to 15 mmHg for 4 hours, trimellitic anhydride was added to the reaction vessel at a concentration of 1 mol% relative to the total resin components, and the mixture was reacted at 180°C and atmospheric pressure for 3 hours to obtain [amorphous polyester resin B-4]. The weight-average molecular weight of the obtained [amorphous polyester resin B-4] was 6000.
[0287] <Synthesis of amorphous polyester resin B-0> In a four-necked flask equipped with a nitrogen inlet tube, a dehydration tube, a stirrer, and a thermocouple, bisphenol A ethylene oxide 2 molar adduct, bisphenol A propylene oxide 2 molar adduct, terephthalic acid, and adipic acid were added, with the molar ratio of bisphenol A propylene oxide 2 molar adduct to bisphenol A ethylene oxide 2 molar adduct being 60 / 40 (bisphenol A propylene oxide 2 molar adduct / bisphenol A ethylene oxide 2 molar adduct), and terephthalic acid and adipic acid. The terephthalic acid and adipic acid were charged in a molar ratio (terephthalic acid / adipic acid) of 97 / 3, and the molar ratio of hydroxyl groups to carboxyl groups (OH / COOH) was 1.3. This mixture was reacted with titanium tetraisopropoxide (500 ppm relative to the resin components) at atmospheric pressure and 230°C for 8 hours, followed by a further reaction under reduced pressure of 10 mmHg to 15 mmHg for 4 hours. Then, trimellitic anhydride was added to the reaction vessel in a ratio of 1 mol% relative to the total resin components, and the mixture was reacted at 180°C and atmospheric pressure for 3 hours to obtain [amorphous polyester resin B-0]. The weight-average molecular weight of the obtained [amorphous polyester resin B-0] was 7000.
[0288] <Preparation of Masterbatch (MB)> 1,200 parts water, 500 parts carbon black (Dexa, Printex35) [DBP oil absorption = 42 mL / 100 mg, pH = 9.5], and 500 parts [amorphous polyester resin B-1] were added and mixed in a Henschel mixer (Nippon Coke Industries Co., Ltd.). The mixture was kneaded at 150°C for 30 minutes using two rolls, then rolled and cooled, and pulverized in a pulperizer to obtain [masterbatch MB-1].
[0289] <Introduction of polyethylene terephthalate (PET)> Flake-shaped recycled PET (manufactured by Kyoei J&T Environmental Co., Ltd.) was mixed with the above-mentioned materials [amorphous polyester resin (B-1) to (B-0)] in order to achieve the solid content ratio shown in Table 1.
[0290] (Example 1) <Preparation of the oil phase> 830 parts of [amorphous polyester resin B-1], 20 parts of the recycled PET, and 100 parts of [masterbatch MB-1] (pigment) were placed in a container and mixed at 5,000 rpm for 60 minutes using a TK homomixer (manufactured by Primix Corporation) to obtain [oil phase 1]. The above proportions indicate the amount of solids in each raw material.
[0291] <Preparation of the aqueous phase> 990 parts water, 20 parts sodium dodecyl sulfate, and 90 parts ethyl acetate were mixed and stirred to obtain a milky white liquid. This was designated as [Aqueous Phase 1].
[0292] <Emulsification> [Oil phase 1] 700 parts were mixed in a TK homomixer at a rotation speed of 8,000 rpm while 20 parts of 28% ammonia water were added and mixed for 10 minutes. Then, 1,200 parts of [Aqueous phase 1] were gradually added dropwise to obtain [Emulsified slurry 1].
[0293] <Solvent removal> [Emulsified slurry 1] was placed in a container equipped with a stirrer and thermometer, and after desolvation at 30°C for 180 minutes, [Desolvent-removed slurry 1] was obtained.
[0294] <Preparation of resin for shells> [Solvent-free slurry 5] was prepared in the same manner as described in Example 1, except that [amorphous polyester resin B-1] was replaced with [amorphous polyester resin B-0] in the preparation of the oil phase described in Example 1. Fifty parts of 3% magnesium chloride solution were added dropwise to [Solvent-removing slurry 1] and stirred for a further 5 minutes. The temperature was then raised to 50°C, [Solvent-removing slurry 5] was added, another 50 parts of 3% magnesium chloride solution were added dropwise, and stirred for a further 5 minutes. After cooling, [Shell A-1] was obtained as the resin for the shell.
[0295] <Agglutination> To 1500 parts of [Solvent-removing slurry 1], 100 parts of 3% magnesium chloride solution were added dropwise and stirred for a further 5 minutes. The temperature was then raised to 60°C, and when the particle size reached 5.0 μm, 100 parts of [Shell A-1] were added dropwise, followed by another 100 parts of 3% magnesium chloride solution, and stirred for a further 5 minutes. The temperature was then raised to 65°C, and 50 parts of sodium chloride were added to complete the flocculation process and obtain [Flocculated slurry 1].
[0296] <Fusion> [Agglomerated slurry 1] was heated to 70°C while stirring, and cooled when it reached the desired average circularity of 0.957 to obtain [Dispersed slurry 1].
[0297] <Washing and drying> [Dispersed slurry 1] After 100 parts were filtered under reduced pressure, the following operations (1) to (4) were performed. (1): 100 parts of deionized water were added to the filter cake, mixed with a TK homomixer (rotating at 12,000 rpm for 10 minutes), and then filtered. (2): 100 parts of a 10% sodium hydroxide aqueous solution were added to the filtered cake from (1), mixed in a TK homomixer (at 12,000 rpm for 30 minutes), and then filtered under reduced pressure. (3): 100 parts of 10% hydrochloric acid were added to the filtered cake from (2), mixed in a TK homomixer (at 12,000 rpm for 10 minutes), and then filtered. (4): 300 parts of deionized water were added to the filtration cake from (3), mixed with a TK homomixer (at 12,000 rpm for 10 minutes), and then filtered.
[0298] The above steps (1) to (4) were repeated twice to obtain [filtered cake 1]. [Filter cake 1] was dried in a circulating air dryer at 45°C for 48 hours, and then sieved through a mesh with a mesh opening of 75 μm to obtain [resin particles 1] which will become toner matrix particles.
[0299] <External additive treatment process> [Resin Particles 1] was mixed with 2.0 parts of hydrophobic silica (Clariant Co., Ltd., HDK-2000) as an external additive in a Henschel mixer, and the mixture was passed through a 500 μm mesh sieve to obtain [Toner 1].
[0300] Except for changing the types and amounts of added resin, shell resin, recycled PET, and MB as shown in Table 1, [Resin Particle 2] to [Resin Particle 8] were prepared in the same manner as [Resin Particle 1], and [Toner 2] to [Toner 8] were prepared in the same manner as [Toner 1]. [Toner 2] to [Toner 4] were designated as Examples 2 to 4, and [Toner 5] to [Toner 8] were designated as Comparative Examples 1 to 4.
[0301] The environmental compatibility, durability, and low-temperature fixation properties of the toners in Examples 1-4 and Comparative Examples 1-4 were evaluated. The conditions for each evaluation are shown below. The results are shown in Table 1.
[0302] <Particle size of resin particles (toner)> The particle size of the resin particles (toner) was measured using a Coulter Multisizer III (manufactured by Coulter). The measurement of the resin particle size was performed as follows:
[0303] First, 2 mL of a surfactant (sodium dodecylbenzenesulfonate, manufactured by Tokyo Chemical Industry Co., Ltd.) was added as a dispersant to 100 mL of electrolyte. The electrolyte was prepared as an approximately 1% NaCl aqueous solution using primary sodium chloride, and ISOTON-II (manufactured by Coulter) was used. To the mixture of electrolyte and surfactant, 10 mg of the sample was added in solid form to obtain an electrolyte in which the sample was suspended.
[0304] The electrolyte containing the suspended sample was dispersed in an ultrasonic disperser for approximately 1 to 3 minutes. Using a Coulter Multisizer III with a 100 μm aperture, the volume and number of toner particles were measured, and the volume and number distributions were calculated. From the obtained distributions, the volume-average particle size (Dv) of the toner was determined.
[0305] <Average particle diameter, average circularity> A flow-type particle image analyzer (FPIA-3000, manufactured by Sysmex Corporation) was used to measure the average particle diameter and average circularity of the resin particles (toner).
[0306] The specific measurement method involved adding 0.1 to 0.5 ml of a surfactant, preferably alkylbenzene sulfonate, as a dispersant to 100 to 150 ml of water from which impurities had been removed beforehand, and then adding approximately 0.1 to 0.5 g of the sample to be measured. The suspension containing the dispersed sample was subjected to dispersion treatment using an ultrasonic disperser for approximately 1 to 3 minutes, and the average particle size, average circularity, and standard deviation (SD) of the circularity were measured using an instrument at a dispersion concentration of 3,000 to 10,000 particles / μL.
[0307] However, the particle diameter was defined as the equivalent diameter of a circle, the average particle diameter was determined by the equivalent diameter of a circle (based on the number of particles), and the analysis conditions for the flow-type particle image analyzer were as follows. Particle size limit: 0.5 μm ≤ Equivalent circle diameter (based on number of particles) ≤ 200.0 μm Particle shape limitation: 0.93 < Circularity ≤ 1.00
[0308] Furthermore, in this embodiment, the definition of average circularity is as follows: (Average circularity) = (Perimeter of a circle equal to the projected area) / (Perimeter of the projected image)
[0309] <Measuring molecular weight> The molecular weights of the resins [B-0] to [B-4] in Table 1 were measured using the following method.
[0310] Gel permeation chromatography (GPC) measurement device: (Tosoh Corporation, GPC-8220GPC) Column: TSKgel SuperHZM-H 15cm 3-row (manufactured by Tosoh Corporation) Temperature: 40℃ Solvent: THF Flow rate: 0.35mL / min Sample: Inject 100 μL of 0.15 mass% of the sample. Sample preparation: Each resin was dissolved in tetrahydrofuran THF (containing stabilizer, manufactured by Wako Pure Chemical Industries) at a concentration of 0.15% by mass. The solution was then filtered through a 0.2 μm filter, and the filtrate was used as the sample. 100 μL of the THF sample solution was injected and measured.
[0311] For measuring the molecular weight of the sample, the molecular weight distribution of the sample was calculated from the relationship between the logarithm of a calibration curve prepared using several monodisperse polystyrene standard samples and the count.
[0312] For calibration curve preparation, ShowdexSTANDARD (manufactured by Showa Denko Corporation) Std. Nos. S-7300, S-210, S-390, S-875, S-1980, S-10.9, S-629, S-3.0, and S-0.580 were used as standard polystyrene samples. An RI (refractive index) detector was used.
[0313] <Method for analyzing toner components> The mass ratios and molar ratios of plant-derived alcohol monomer units, PET-derived monomer units, and non-plant-derived monomer units (excluding PET) in the resin constituting each toner were determined by separation using gel permeation chromatography (GPC), and the separated components were calculated and qualitatively evaluated using the analytical methods described below.
[0314] The qualitative evaluation based on the above analysis was performed by estimating the main components from the soft decomposition of ester bonds in the resin structure by methylation using gas chromatography-mass spectrometry (GC / MS) at 300°C with a reaction reagent (10% Tetramethyl ammonium hydroxide (TMAH) / Methanol solution).
[0315] <Measurement of plant-derived component percentage> One g each of the resins [B-1] to [B-4] and [A-1] to [A-5] from Table 1 was added to 100 mL of chloroform, and the soluble components were dissolved under conditions of 25°C for 30 minutes with stirring to obtain a solution. This solution was filtered through a membrane filter with a mesh size of 0.2 μm to obtain the chloroform-soluble components of each resin. The chloroform-soluble component was dried at 45°C for 24 hours, and the resulting CO2 (carbon dioxide) was burned to obtain C (graphite). Radioactive carbon isotopes of C (graphite) 14 The C concentration was measured using an accelerator mass spectrometer (AMS, manufactured by Beta Analytic). Measured 14 The percentage of plant-derived components was calculated by substituting the C concentration into the following formula. Percentage of plant-derived components in each resin (%) = 14 C concentration (pMC) / 107.5×100...Equation (1)
[0316] Using the plant-derived component percentage values obtained above, the amounts of plant-derived monomer units and plant-derived alcohol monomer units in each resin were determined.
[0317] <Shell thickness> The prepared toner was embedded in epoxy resin and cured. Ultrathin sections (approximately 100 nm thick) of the toner were prepared using an ultramicrotome (Leica ULTRACUT UCT, using a diamond knife).
[0318] The sample was gas-exposed with ruthenium tetroxide, osmium tetroxide, or another stain to differentiate between the core and shell layers. The exposure time was adjusted as needed based on the contrast observed. Subsequently, the sample was observed using a transmission electron microscope (TEM) (JEM-2100, JEOL) at an acceleration voltage of 100 kV.
[0319] Furthermore, compositional contrast was imparted by other means such as selective etching, and the core and shell layers were evaluated by observation with a transmission microscope after pretreatment. Domain particles were found in the shell layers of Examples 1-4 and Comparative Examples 1-3, but no domain particles were observed in the shell layer of Comparative Example 4.
[0320] The cross-sectional images of the observed toner were binarized using commercially available image processing software (Image-Pro Plus 5.1, Media Cybernetics) to calculate the average equivalent diameter of the resin particles in the core-shell structure and the average equivalent diameter of the core. Twenty toner cross-sections were observed, and the average equivalent diameter was determined. The shell thickness was calculated using the following formula. Shell thickness = Average equivalent diameter of resin particles in the core-shell structure / Average equivalent diameter of the core
[0321] <Analysis of the resin composition of the surface layer> To confirm that the resin particles or toner surface contain resin components such as plant-derived alcohol monomer units or PET-derived monomer units, this was confirmed by surface composition analysis using nanoIR. The composition was obtained by acquiring the IR spectrum of the surface layer of the fine particles using an analytical technique that achieves nanoscale resolution by combining AFM and IR of nanoIR. This analysis identified whether plant-derived alcohol monomer units and PET-derived monomer units were present in the surface layer. The ratio of the signal peak intensity of non-plant-derived monomer units (excluding PET) to the sum of the signal peak intensities of plant-derived alcohol monomer units and PET-derived monomer units was determined for the outermost resin layer when the shell layer was divided into 10 equal parts in the volume-average particle size direction of each resin particle or toner. The results are shown in Table 1.
[0322] [Table 1]
[0323] The environmentally friendly resin ratios for the resins [B-1] to [B-4] and [A-1] to [A-5] in Table 1 were used to determine the amount of environmentally friendly components present in the core and shell, thereby calculating the environmentally friendly ratio and assessing the environmental impact. The criteria for judgment are as follows:
[0324] <Environmental compatibility> [Evaluation Criteria] ◎: The core and shell resins contain 20% or more plant-derived alcohol monomer units, and the PET content in the amorphous resin of the shell is 20% or more. ○: The core resin contains 5% or more plant-derived alcohol monomer units, and the shell resin contains 2% or more plant-derived alcohol monomer units. ×: The core resin contains less than 5% plant-derived alcohol monomer units, or the shell resin contains less than 2% plant-derived alcohol monomer units.
[0325] <Heat-resistant storage stability> To evaluate thermal preservation properties, toners from Examples 1-4 and Comparative Examples 1-4 were filled into glass containers and left in a constant temperature bath at 50°C for 24 hours. Each toner was cooled to 24°C, and the penetration rate was measured using a penetration test (JIS K2235-1991). The criteria for determining thermal preservation properties based on penetration rate are as follows. ○…25mm or more △…10~25mm ×...less than 10mm
[0326] Although embodiments of the present invention have been described above, the present invention is not limited to any particular embodiment, and various modifications and changes are possible within the scope of the invention as described in the claims.
[0327] Examples of embodiments of the present invention include the following: <1> Resin particles having a core-shell structure comprising a first resin and a second resin, The first resin contains, in 100 mol% of alcohol monomer units, 5 mol% to 30 mol% of plant-derived alcohol monomer units. The second resin contains, in 100 mol% of alcohol monomer units, 2 mol% to 30 mol% of plant-derived alcohol monomer units. Resin particles characterized in that, in the outermost resin when the shell layer in the core-shell structure is divided into 10 equal parts in the diametrical direction, the signal peak intensity of monomer units of non-plant-derived resins other than PET and PBT is 5 times or more than the sum of the signal peak intensity of plant-derived alcohol monomer units obtained by nano IR measurement and the signal peak intensity of monomer units derived from at least one of PET and PBT. <2> The amount of PET and / or PBT-derived material contained in 100% by mass of the second resin is 40% by mass or less. <1> The resin particles described above. <3> The shell layer contains domain particles, and the domain particles contain the resin contained in the core in the core-shell structure, <1> or <2> The resin particles described above. <4> The thickness of the shell layer is such that (average circular equivalent diameter of the resin particles of the core-shell structure / average circular equivalent diameter of the core) = 1.005 or more and 1.5 or less. <1> , <2> or <3> The resin particles described above. <5> The aforementioned <1> , <2> , <3> ,or <4> A toner characterized by containing the resin particles described above. <6> The aforementioned <5> A developer characterized by containing the toner described above. <7> The aforementioned <6> A toner storage unit characterized by housing the toner described in [the relevant document].
[0328] The aforementioned <1> from <4> Resin particles as described in any of the above <5> The toner described above, <6> The developer described above, <7> The toner storage unit described above can solve the aforementioned problems in the conventional method and achieve the objectives of the present invention. [Prior art documents] [Patent Documents]
[0329] [Patent Document 1] Japanese Patent Publication No. 2017-111416 [Patent Document 2] Japanese Patent Publication No. 2015-025851
Claims
1. A resin particle having a core-shell structure comprising a core containing a first resin and a shell layer containing a second resin that covers at least a portion of the surface of the core, The first resin is an amorphous polyester resin containing 5 mol% to 30 mol% of plant-derived alcohol monomer units in a 100 mol% alcohol monomer unit ratio. The second resin is an amorphous polyester resin containing 2 mol% to 30 mol% of plant-derived alcohol monomer units in 100 mol% of alcohol monomer units. The first resin and / or the second resin comprises monomer units derived from PET and / or PBT. Resin particles characterized in that, in the outermost resin when the shell layer in the core-shell structure is divided into 10 equal parts in the diametrical direction, the signal peak intensity of monomer units of non-plant-derived resins excluding PET and PBT is 5 times or more than the sum of the signal peak intensity of plant-derived alcohol monomer units obtained by nano IR measurement and the signal peak intensity of monomer units derived from PET and / or PBT.
2. The resin particles according to claim 1, wherein the content of monomer units derived from PET and / or PBT in 100% by mass of the second resin is 40% by mass or less.
3. The resin particle according to claim 1 or 2, wherein the shell layer contains domain particles, and the domain particles contain the resin contained in the core in the core-shell structure.
4. The resin particle according to claim 1 or 2, wherein the thickness of the shell layer is (average circular equivalent diameter of the resin particles of the core-shell structure / average circular equivalent diameter of the core) = 1.005 or more and 1.5 or less.
5. A toner characterized by containing resin particles as described in claim 1 or 2.
6. A developer characterized by containing the toner described in claim 5.
7. A toner storage unit characterized by storing the toner described in claim 5.
Citation Information
Patent Citations
Sustainable toner
JP2014098149A
Manufacturing method of toner
JP2015025851A
Toner comprising sustainable polyester resin
JP2015081348A
Production method of toner for electrostatic charge image development
JP2017111416A
Polyester resin, method for manufacturing same, and coating
WO2022202672A1