Spunbond nonwoven fabric and method for manufacturing the same

A spunbond nonwoven fabric with enhanced strength and flexibility is achieved through core-sheath composite fibers with specific polypropylene resin components, addressing the limitations of existing fabrics in strength and basis weight.

JP7948039B2Active Publication Date: 2026-11-11TORAY INDUSTRIES INC
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
JP2023037293
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-03-10
Publication Date
2026-11-11
Estimated Expiration
2043-03-10

AI Technical Summary

Technical Problem

Existing spunbond nonwoven fabrics face challenges in achieving high strength while maintaining low basis weight, flexibility, and texture, as methods to improve strength often result in insufficient thermal adhesion or fiber strength.

Method used

A spunbond nonwoven fabric composed of core-sheath composite fibers with specific polypropylene resin components, including a core component with a branching index of 0.950 to 0.990 and isotactic pentad fraction of 0.950 to 0.995, and a sheath component with controlled melting peak temperatures, is produced using a spinning process that includes cooling, solidification, and stretching at specific speeds.

Benefits of technology

The resulting fabric exhibits higher strength, flexibility, and texture, making it suitable for environmentally friendly applications such as disposable diapers and masks, despite reduced plastic usage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007948039000001
    Figure 0007948039000001
Patent Text Reader

Abstract

To provide a spun-bonded nonwoven fabric having excellent strength even with low basis weight, excellent in flexibility and touch.SOLUTION: A spun-bonded nonwoven fabric includes a core-sheath type conjugate fiber composed of a core component and a sheath component, having a fused part and a non-fused part. The core component is a polypropylene-based resin having a branch index g of 0.950 or more and 0.990 or less, and an isotactic pentad ratio (mmmm) of 0.950 or more and 0.995 or less. The sheath component is a polypropylene-based resin.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a spunbond nonwoven fabric.

Background Art

[0002] Spunbond nonwoven fabrics are widely used in sanitary materials such as disposable diapers and sanitary napkins, as well as in masks, due to their low cost and the ease of obtaining appropriate flexibility and physical properties for practical use. In these applications, the products are often discarded after a single use, followed by incineration or landfill disposal. From the perspective of environmental consideration, there is a demand for reducing the amount of plastic used.

[0003] Reducing the amount of plastic in a spunbond nonwoven fabric specifically refers to the nonwoven fabric mass per 1 m 2 , that is, the basis weight (g / m 2 )) to be reduced. However, as the basis weight is reduced, the tensile strength of the nonwoven fabric generally decreases, making it more prone to tearing during practical use. Accordingly, various studies have been conducted on methods for improving the strength of spunbond nonwoven fabrics.

[0004] In general, two possible methods can be considered for improving the strength of a spunbond nonwoven fabric: a method of improving the strength of the constituent fibers themselves, and a method of increasing the number of adhesion points between the constituent fibers. As for the former, for example, Patent Document 1 proposes adding a specific amount of a polypropylene resin having a molecular weight distribution (Mw / Mn) and an MFR within specific ranges, in which the proportion of reverse-inserted propylene units is kept below a certain level, and which further has a specific melt strength. It is described that both the tenacity and the ease of elongation of the yarn can be achieved. As for the latter, for example, Patent Document 2 proposes reducing the crystallite size by controlling the melt mass flow rate of the polypropylene resin and the spinning conditions, so as to set the melting point and the heat of fusion within specific ranges. It is described that this improves the thermal adhesiveness in the manufacturing process of the spunbond nonwoven fabric.

Prior Art Documents

Patent Documents

[0005] [Patent Document 1] Special Publication No. 2008-523231 [Patent Document 2] Japanese Patent Publication No. 2019-196576 [Overview of the Initiative] [Problems that the invention aims to solve]

[0006] However, while the method disclosed in Patent Document 1 can improve the strength of the yarn to some extent, when used in the fibers constituting a spunbond nonwoven fabric, the amount of high melt-strength polypropylene added is relatively small, which tends to result in insufficient thermal adhesion. Therefore, the strength of the spunbond nonwoven fabric does not become that high.

[0007] On the other hand, while the method disclosed in Patent Document 2 can improve heat adhesion to some extent and produce a spunbond nonwoven fabric with a certain strength, the fiber strength tends to be somewhat low because the crystallite size is not sufficiently large, and there is still room for improvement in the strength of the spunbond nonwoven fabric. Therefore, the objective of the present invention is to provide a spunbond nonwoven fabric that has excellent strength even at low basis weight, as well as excellent flexibility and texture. [Means for solving the problem]

[0008] As a result of diligent research to achieve the above objective, the inventors have found that by setting the branching index g of the polypropylene resin fibers constituting the spunbond nonwoven fabric to a specific range, the strength of the fibers constituting the spunbond nonwoven fabric can be improved, and a spunbond nonwoven fabric with higher strength than before can be obtained.

[0009] This invention was completed based on these findings, and according to this invention, the following inventions are provided.

[0010] [1] A spunbond nonwoven fabric comprising a core-sheath composite fiber consisting of a core component and a sheath component, wherein the core component is a polypropylene resin having a branching index g of 0.950 or more and 0.990 or less and an isotactic pentad fraction (mmmm) of 0.950 or more and 0.995 or less, and the sheath component is a polypropylene resin, and the spunbond nonwoven fabric has fused portions and unfused portions.

[0011] [2] The spunbond nonwoven fabric according to [1], wherein the orientation parameter Oc of the core component of the core-sheath type composite fiber in the non-fused portion is 5.0 or more and 8.0 or less.

[0012] [3] The spunbond nonwoven fabric according to [1] or [2], wherein the ratio Oc / Os of the orientation parameter Oc of the core component to the orientation parameter Os of the sheath component of the core-sheath composite fiber in the non-fused portion is 1.2 or more and 2.0 or less.

[0013] [4] The spunbond nonwoven fabric according to any of [1] to [3] above, wherein the melting peak temperature Tms(°C) of the sheath component and the melting peak temperature Tmc(°C) of the core component of the core-sheath composite fiber satisfy the following formula 1. Tmc-30≦Tms≦Tmc-5 (Equation 1).

[0014] [5] A process to obtain a core-sheath composite fiber, comprising: spinning a polypropylene resin as the core component, having a branching index g of 0.950 or more and an isotactic pentad fraction (mmmm) of 0.950 or more and a sheath component, from a composite spinneret having an ejection hole; cooling and solidifying the spun yarn; and pulling and stretching it with an ejector at a spinning speed of 3500 m / min or more and 6500 m / min or less; The process involves collecting the core-sheath composite fibers onto a net to form a fiber web, The process of heat-bonding the aforementioned fiber web, A method for producing a spunbond nonwoven fabric having [the specified characteristics]. [Effects of the Invention]

[0015] According to the present invention, a spunbond nonwoven fabric with higher strength than conventional spunbond nonwoven fabrics can be obtained. Therefore, even if a spunbond nonwoven fabric with a relatively low basis weight is used, it will have excellent physical properties, and furthermore, it will be possible to produce a spunbond nonwoven fabric with excellent flexibility and feel. As a result, it can be suitably used as an environmentally friendly spunbond nonwoven fabric with reduced plastic raw materials for sanitary materials such as disposable diapers and sanitary napkins, as well as masks and the like. [Modes for carrying out the invention]

[0016] The spunbond nonwoven fabric of the present invention is a spunbond nonwoven fabric composed of core-sheath type composite fibers consisting of a core component and a sheath component, wherein the core component is a polypropylene resin having a branching index g of 0.950 or more and 0.990 or less and an isotactic pentad fraction (mmmm) of 0.950 or more and 0.995 or less, and the sheath component is a polypropylene resin having fused portions and unfused portions. In this way, as described above, even with a relatively low basis weight, it is possible to obtain a spunbond nonwoven fabric that has excellent physical properties and furthermore, excellent flexibility and texture.

[0017] The components of this invention will be described in detail below, but the present invention is not limited in any way to the scope described below, as long as it does not exceed the gist of the invention.

[0018] [Core-sheath type composite fiber] The core-sheath composite fiber constituting the spunbond nonwoven fabric of the present invention has a core and sheath component that are both made of polypropylene resin. Here, "polypropylene resin" refers to a resin having propylene units as repeating units, and includes propylene homopolymers or copolymers of propylene and various α-olefins. Among these, propylene homopolymers are preferred in order to prevent a decrease in spinning stability and strength.

[0019] In particular, the polypropylene resin preferably contains 60% by mass or more of propylene homopolymer, more preferably 70% by mass or more, and even more preferably 80% by mass or more. This allows for maintaining good spinnability and improving strength.

[0020] This polypropylene-based resin may be a mixture of two or more types, and a resin composition containing polyethylene, other olefin-based resins such as poly-4-methyl-1-pentene, or thermoplastic elastomers may also be used.

[0021] The polypropylene resin used in the present invention may, as necessary, contain additives such as commonly used antioxidants, weather stabilizers, light stabilizers, heat stabilizers, antistatic agents, antistatic aids, fogging agents, antiblocking agents, lubricants including polyethylene wax, crystal nucleating agents, and pigments, or other polymers, to further enhance the effects of the present invention or to impart other properties, provided that such additives do not impair the effects of the present invention.

[0022] Furthermore, this polypropylene resin may contain a fatty acid amide compound with 23 to 50 carbon atoms to improve slipperiness and flexibility. By preferably setting the number of carbon atoms of the fatty acid amide compound mixed into the polypropylene resin to 23 or more, and more preferably to 30 or more, excessive exposure of the fatty acid amide compound to the fiber surface is suppressed, resulting in excellent spinnability and processing stability, and maintaining high productivity. On the other hand, by preferably setting the number of carbon atoms of the fatty acid amide compound to 50 or less, and more preferably to 42 or less, the fatty acid amide compound can easily move to the fiber surface, thereby imparting slipperiness and flexibility to the spunbond nonwoven fabric.

[0023] Examples of fatty acid amide compounds with 23 to 50 carbon atoms used in the present invention include saturated fatty acid monoamide compounds, saturated fatty acid diamide compounds, unsaturated fatty acid monoamide compounds, and unsaturated fatty acid diamide compounds.

[0024] Specifically, examples of fatty acid amide compounds with 23 to 50 carbon atoms include tetradocosanoamide, hexadocosanoamide, octadocosanoamide, nervonamide, tetracosapentaenoamide, hernamide, ethylenebislauric acidamide, methylenebislauric acidamide, ethylenebisstearateamide, ethylenebishydroxystearateamide, ethylenebisbehenamide, hexamethylenebisstearateamide, hexamethylenebisbehenamide, hexamethylenehydroxystearateamide, distearyladipamide, distearylsebacinamide, ethylenebisoleamide, ethylenebiserucamide, and hexamethylenebisoleamide, and several of these can be used in combination. Among these, ethylenebisstearateamide is preferred because its excellent thermal stability allows for melt spinning, and it is possible to obtain a spunbond nonwoven fabric with excellent slipperiness and flexibility while maintaining high spinning stability.

[0025] In the present invention, it is preferable that the amount of fatty acid amide compound contained in the polypropylene resin constituting the core-sheath composite fiber (hereinafter sometimes simply referred to as the fatty acid amide compound content) is 0.01% to 5% by mass. By setting the fatty acid amide compound content to 0.01% by mass or more, more preferably 0.1% by mass or more, appropriate slipperiness and flexibility can be provided. On the other hand, by setting the fatty acid amide compound content to 5% by mass or less, more preferably 3% by mass or less, and even more preferably 1% by mass or less, a decrease in spinnability can be suppressed.

[0026] The fatty acid amide compound content referred to here is the ratio (%) of the mass of the fatty acid amide compound to the total mass of the polypropylene resin fiber. In other words, for example, even if the aforementioned fiber is a core-sheath type composite fiber and the fatty acid amide compound is contained only in the sheath component of this core-sheath type composite fiber, the ratio of the mass of the fatty acid amide compound to the total mass of the core-sheath type composite fiber will be calculated.

[0027] One method for measuring the content of these fatty acid amide compounds is to extract the additive from the fibers using a solvent and then quantitatively analyze it using liquid chromatography-mass spectrometry (LS / MS). The extraction solvent is appropriately selected depending on the type of fatty acid amide compound, but for example, in the case of ethylenebisstearamide, one method is to use a chloroform-methanol mixture.

[0028] The melting point (Tm) of the polypropylene resin used in this invention is preferably 120°C to 200°C for both the core component and the sheath component. By setting the lower limit of this melting point (Tm) range to preferably 120°C or higher, more preferably 130°C or higher, and even more preferably 140°C or higher, it becomes easier to obtain heat resistance that is suitable for practical use. Furthermore, by setting the upper limit of the above melting point range to preferably 200°C or lower, more preferably 180°C or lower, and even more preferably 170°C or lower, it becomes easier to cool the yarn extruded from the die, suppressing fusion between fibers and facilitating stable spinning even with thin fiber diameters.

[0029] The melting point (Tm) of the polypropylene resin mentioned above refers to the maximum melting peak temperature measured and calculated using the differential scanning calorimetry (DSC) method described below. (1) Sample 0.5 mg to 5 mg of polypropylene resin. (2) Using differential scanning calorimetry (DSC), the temperature is increased from room temperature to 200°C at a heating rate of 20°C / min to obtain a DSC curve. (3) Read the peak top temperature of the melting endothermic peak from the DSC curve and define it as the melting peak temperature Tm (°C) of the polypropylene resin.

[0030] The core component of the core-sheath composite fiber according to the present invention is a polypropylene resin having a branching index g of 0.950 or more and 0.990 or less, and an isotactic pentad fraction (mmmm) of 0.950 or more and 0.995 or less. Having such a polypropylene resin as the core component of the core-sheath composite fiber results in a spunbond nonwoven fabric with high strength and excellent productivity.

[0031] First, the core component is a polypropylene resin with a branching index g of 0.950 or more and 0.990 or less. The branching index g of this polypropylene resin is an index indicating the degree of branching of the long chains of the polypropylene resin, and is described, for example, in "Developments in Polymer Characterization-4" (JV Dawkinsed. Applied Science Publishers, 1983). A branching index g of 0.950 or more, preferably 0.965 or more, and more preferably 0.980 or more, prevents the melt tension from becoming too high, and ensures stable spinning without insufficient stretch-following ability during melt spinning and stretching. This is presumed to be because, by including polypropylene with long-chain branching in the main chain skeleton, during cooling and solidification, the long-chain branching promotes the entanglement of amorphous tie molecules that penetrate the microcrystals in the system (pseudo-crosslinking effect between microcrystals), and in the subsequent stretching process, the stretching stress is uniformly transmitted throughout the entire system (tendency toward uniform stretching), thereby reducing voids generated inside the fiber and suppressing yarn breakage. Furthermore, when the branching index g is 0.990 or less, crystallization progresses due to the microcrystal formation effect, and the sheet strength of the spunbond nonwoven fabric is improved by the increase in single-fiber strength.

[0032] In the present invention, the branching index g of the polypropylene resin shall be measured by the following method. (1) Take three samples of 10 mg of polypropylene resin, which is the core component. (2) Dissolve the above sample in 1,2,4-trichlorobenzene. The concentration at this time should be 1 mg / mL. (3) A gel permeation chromatography (GPC) instrument equipped with a differential refractometer (RI) and a viscometer (Viscometer) (for example, Waters' "Alliance GPC / V2000") and GPCV analysis software compatible with the instrument (for example, Waters' "Millennium") 32 Using (etc.), the intrinsic viscosity of the sample is measured under the following measurement conditions. The arithmetic mean of the resulting intrinsic viscosity is rounded to the fourth decimal place and given [η] br Let's assume that. • Mobile phase solvent: 1,2,4-trichlorobenzene ·Flow rate: 1mL / min • Column: Two "GMHHR-H(S)HT" columns manufactured by Tosoh Corporation, connected together. Column temperature, sample injection port temperature, and individual detector temperatures: 140°C • Sample injection volume (sample loop volume): 0.2175 mL for the Waters Alliance GPC / V2000 mentioned above. (4) The weight-average molecular weight of the sample is measured by low-angle laser light scattering photometric measurement. (5) Under the same conditions as in (3), the intrinsic viscosity of a linear polypropylene resin having a weight-average molecular weight equivalent to that obtained in (4) is measured. Alternatively, if it is not possible to measure the intrinsic viscosity of a linear polypropylene resin having a weight-average molecular weight equivalent to that obtained in (4), since it is well known from the Mark-Houwink-Sakurada equation that the logarithm of the intrinsic viscosity of a linear polypropylene resin has a linear relationship with the logarithm of its molecular weight, the intrinsic viscosity of a commercially available linear polypropylene resin (for example, "Novatec PP(registered trademark) FY6" manufactured by Nippon Polypropylene Co., Ltd.) can be measured, and the value can be obtained by appropriately extrapolating its intrinsic viscosity to the low molecular weight or high molecular weight side. The arithmetic mean of the intrinsic viscosity obtained in this way is rounded to the fourth decimal place to obtain [η]. lin Let's assume that. (6) Calculate the branching exponent g from the following formula (1), and round the obtained value to the fourth decimal place.

[0033] g = [η]br / [η] lin ···(1) In general, when a long-chain branched structure is introduced into a polymer molecule, the radius of gyration becomes smaller compared to a linear polymer molecule of the same molecular weight. As the radius of gyration decreases, the intrinsic viscosity decreases. Therefore, as the long-chain branched structure is introduced, the intrinsic viscosity ([η] lin ) of the branched polymer relative to the intrinsic viscosity ([η] br ) of linear polypropylene of the same molecular weight br / [η] lin ), namely the branching index g, tends to decrease.

[0034] Next, the aforementioned core component has an isotactic mesopentad fraction (mmmm) of 0.950 or more and 0.995 or less. It is more preferably 0.965 or more, and particularly preferably 0.980 or more. The isotactic mesopentad fraction (mmmm) is an index indicating the stereoregularity of the crystal phase of polypropylene measured by a nuclear magnetic resonance method (NMR method). A higher value indicates higher stereoregularity, and the crystallinity and melting point become higher. When the isotactic mesopentad fraction of the polypropylene-based resin is 0.950 or more, the high crystallinity improves the yarn strength of the spunbond, and the spunbond nonwoven fabric has mechanical strength that allows practical use. When the isotactic mesopentad fraction is 0.995 or less, the spinnability during melt spinning is maintained, and a spunbond nonwoven fabric can be stably obtained. This is because microcrystal nuclei form preferentially and grow progressively, so even if yarn swaying occurs during finening, the yarns will not fuse with each other even if they come into contact, which suppresses yarn breakage caused by entangling surrounding yarns.

[0035] The isotactic mesopentad fraction (mmmm) is measured by 13 C nuclear magnetic resonance( 13This is the isotactic fraction at the pentad unit level in polypropylene molecular chains, measured using 1C-NMR, and is measured by a well-known method (for example, the method described in A. Zambelli, "Macromolecules," 1973, Vol. 6, p. 625, or ibid., "Macromolecules," 1975, Vol. 8, p. 687). 13 This is measured by the intensity fraction of the [mmmm] peak among the total absorption peaks in the methyl carbon region of the 1C-NMR spectrum.

[0036] Furthermore, the melt flow rate (hereinafter sometimes referred to as MFR) of the polypropylene resin used in the present invention is preferably 10 g / 10 min or more and 850 g / 10 min or less. When the MFR is 10 g / 10 min or more, more preferably 20 g / 10 min or more, and even more preferably 30 g / min or more, even fine fiber diameters can be stably spun, resulting in a spunbond nonwoven fabric with excellent texture and a uniform weave. On the other hand, when the MFR is 850 g / 10 min or less, more preferably 600 g / 10 min or less, and even more preferably 400 g / 10 min or less, a spunbond nonwoven fabric with high strength is obtained.

[0037] Furthermore, the MFR of polypropylene resins will be the value measured according to ASTM D1238 (Method A). According to this standard, polypropylene is to be measured under a load of 2.16 kg and a temperature of 230 °C.

[0038] Furthermore, the MFR of a polypropylene resin can be adjusted by blending two or more polypropylene resins with different MFRs in any proportion. In this case, the MFR of the resin to be blended with the main polypropylene resin is preferably 10 g / 10 min or more, more preferably 20 g / 10 min or more, and even more preferably 30 g / 10 min or more. It is also preferably 1000 g / 10 min or less, more preferably 800 g / 10 min or less, and even more preferably 600 g / 10 min or less. By setting the MFR within the above range, it is possible to suppress partial viscosity variations in the blended polypropylene resin and prevent unevenness in fineness and deterioration of spinnability.

[0039] Furthermore, the MFR can be controlled by the weight-average molecular weight of the polypropylene resin. The higher the weight-average molecular weight of the polypropylene resin, the smaller the MFR. Alternatively, the MFR may be adjusted by adding at least one radical generator from the group consisting of organic peroxides, azo compounds, and nitroxides to the polypropylene resin to decompose it.

[0040] The core-sheath composite fiber according to the present invention satisfies the following equation 1, where the melting peak temperature Tms (°C) of the sheath component and the melting peak temperature Tmc (°C) of the core component are equal. Tmc-30≦Tms≦Tmc-5 (Equation 1).

[0041] Regarding the relationship between the melting peak temperature Tms(°C) of the sheath component and the melting peak temperature Tmc(°C) of the core component of this composite fiber, if the melting peak temperature Tms(°C) of the sheath component of the core-sheath composite fiber is (Tmc-5)°C or less (i.e., in the above formula 1, Tms ≤ (Tmc-5), and so on), preferably (Tmc-7)°C or less, and more preferably (Tmc-10)°C or less, then only the component that forms the fiber surface layer can be softened during heat bonding. By doing so, the orientation of the fiber inner layer can be preserved while the fibers can be strongly heat-bonded to each other, resulting in a spunbond nonwoven fabric with strength suitable for practical use. On the other hand, if the melting peak temperature Tms(°C) of the sheath component of the core-sheath composite fiber is (Tmc-30)°C or higher (i.e., in the above formula 1, (Tmc-30) ≤ Tms, and so on), preferably (Tmc-25)°C or higher, and more preferably (Tmc-20)°C or higher, it is possible to prevent the fiber surface from becoming excessively softened during heat bonding and causing operational problems such as sticking to the heat bonding roll, resulting in a high-quality spunbond nonwoven fabric.

[0042] As the composite form of the core-sheath type composite fiber constituting the spunbond nonwoven fabric of the present invention, for example, composite forms such as concentric core-sheath type, eccentric core-sheath type, and sea-island type can be used. In particular, a core-sheath type composite form is preferred, that is, the composite fiber is a core-sheath type composite fiber, because it has excellent spinnability and the fibers can be uniformly bonded to each other by heat bonding, and a concentric core-sheath type composite form is preferred, that is, the composite fiber is a concentric core-sheath type core-sheath type composite fiber.

[0043] The core-sheath type composite fibers constituting the spunbond nonwoven fabric of the present invention preferably have an average single fiber fineness of 0.3 dtex or more and 3.0 dtex or less. By setting the average single fiber fineness to preferably 0.3 dtex or more, more preferably 0.4 dtex or more, and even more preferably 0.5 dtex or more, a decrease in spinnability can be prevented, resulting in excellent production stability and a high-quality spunbond nonwoven fabric. On the other hand, by setting the average single fiber fineness to preferably 3.0 dtex or less, more preferably 2.0 dtex or less, and even more preferably 1.5 dtex or less, a spunbond nonwoven fabric with excellent texture, uniform texture, and strength can be obtained. The average single fiber fineness can be controlled by the spinning temperature, single-hole discharge amount, spinning speed, etc., as described later.

[0044] The core-sheath type composite fibers constituting the spunbond nonwoven fabric of the present invention preferably have an average single fiber diameter of 8 μm or more and 20 μm or less. By having an average single fiber diameter of preferably 8 μm or more, more preferably 9 μm or more, and even more preferably 10 μm or more, a decrease in spinnability can be prevented, resulting in excellent production stability and a high-quality spunbond nonwoven fabric. On the other hand, by having an average single fiber diameter of preferably 20 μm or less, more preferably 17 μm or less, and even more preferably 14 μm or less, a spunbond nonwoven fabric with excellent texture, uniform texture, and superior strength can be obtained.

[0045] In this invention, the average single fiber diameter (μm) of the core-sheath type composite fiber shall be the value obtained by measuring and calculating it according to the following procedure. (1) Take 10 small sample pieces (100 x 100 mm) randomly from the spunbond nonwoven fabric. (2) Take surface photographs at 500x to 2000x magnification using a microscope or scanning electron microscope, and measure the width (diameter) of 10 composite fibers in the non-fused portion from each sample, for a total of 100 fibers. If the cross-section of the composite fiber is irregular, measure the cross-sectional area and determine the diameter of a perfect circle with the same cross-sectional area. (3) The average of the diameter values ​​of the 100 measured fibers is calculated and rounded to the second decimal place to obtain the average single fiber diameter (μm).

[0046] Furthermore, the average single fiber diameter can be controlled by the spinning temperature, single-hole extrusion rate, spinning speed, etc., as described later. In the spunbond nonwoven fabric of the present invention, it is preferable that the mass ratio of the sheath component is 20% by mass or more and 80% by mass or less. When the mass ratio of the sheath component is preferably 20% by mass or more, more preferably 30% by mass or more, and even more preferably 40% by mass or more, the sheath components fuse firmly to each other during heat bonding, resulting in a spunbond nonwoven fabric with sufficient strength for practical use. On the other hand, when the ratio of the sheath component is preferably 80% by mass or less, more preferably 70% by mass or less, and even more preferably 60% by mass or less, the single-fiber strength of the composite fibers is improved, resulting in a spunbond nonwoven fabric with sufficient strength for practical use.

[0047] The cross-sectional shape of the composite fibers constituting the spunbond nonwoven fabric of the present invention can be a round cross-section, a flat cross-section, or an irregular cross-section such as a Y-shape or a C-shape. Among these, a round cross-section is preferred because it does not have the structural difficulty in bending that flat or irregular cross-sections have, and a spunbond nonwoven fabric with excellent flexibility can be obtained. A hollow cross-section can also be used as the cross-sectional shape, but a solid cross-section is preferred because it has excellent spinnability and can be stably spun even with a thin fiber diameter.

[0048] [Spunbond nonwoven fabric] The spunbond nonwoven fabric of the present invention is a spunbond nonwoven fabric composed of the aforementioned core-sheath type composite fibers. Furthermore, the spunbond nonwoven fabric of the present invention has fused portions and non-fused portions. This configuration results in a spunbond nonwoven fabric that has sufficient strength for practical use while maintaining flexibility and a pleasant feel. Here, the fused portions refer to areas where the core-sheath type composite fibers are fused together, and the non-fused portions refer to areas where the core-sheath type composite fibers are not fused together and maintain their cross-sectional shape.

[0049] In the spunbond nonwoven fabric of the present invention, the orientation parameter Oc of the core component of the non-fused portion is preferably 5.0 or more and 8.0 or less. By having an orientation parameter of the core component preferably 5.0 or more, more preferably 5.1 or more, and even more preferably 5.2 or more, the strength of the inner layer of the fibers is improved, resulting in a spunbond nonwoven fabric with strength suitable for practical use after heat bonding. Furthermore, operational problems such as the fiber surface layer becoming excessively softened and sticking to the heat roll during heat bonding can be prevented. On the other hand, by having an orientation parameter Oc of the core component of the core-sheath type composite fiber in the non-fused portion preferably 8.0 or less, more preferably 7.9 or less, and even more preferably 7.8 or less, a spunbond nonwoven fabric with excellent flexibility is obtained. Furthermore, since excessive tensile stress concentration in the inner layer of the fibers during spinning is suppressed, spinning stability can be improved, resulting in a spunbond nonwoven fabric with flexibility suitable for use as a nonwoven fabric for sanitary materials and with excellent strength. The orientation parameter Oc of the core component of the core-sheath type composite fiber in the non-fused portion can be controlled by the MFR of the polypropylene resin, the melting point, the additives, the mass ratio of the sheath component of the core-sheath type composite fiber, and / or the spinning temperature and spinning speed described later.

[0050] In the spunbond nonwoven fabric of the present invention, the orientation ratio (Oc / Os) of the orientation parameter Os of the sheath component to the orientation parameter Oc of the core component of the non-fused portion is preferably 1.2 or more and 2.0 or less. When the orientation ratio (Os / Oc) is preferably 1.2 or more, more preferably 1.3 or more, and even more preferably 1.4 or more, the orientation parameter Os of the sheath component is lower than the orientation parameter Oc of the core component, and only the surface layer of the fibers can be softened during heat bonding. In this way, the molecular orientation of the inner layer of the fibers can be firmly heat-bonded to each other while retaining the molecular orientation, resulting in a spunbond nonwoven fabric with strength suitable for practical use. On the other hand, when the orientation ratio (Oc / Os) is preferably 2.0 or less, and more preferably 1.9 or less, it is possible to prevent excessive stress concentration in the inner layer of the fibers during spinning, which reduces spinning stability, resulting in a spunbond nonwoven fabric with excellent strength and high quality.

[0051] Here, the orientation parameter Oc of the core component or the orientation parameter Os of the sheath component of the core-sheath type composite fiber in the present invention is an index (unitless) in which a larger value indicates that the molecular chains are oriented in a specific direction, and a smaller value indicates that the molecular chains are oriented randomly. Note that this orientation parameter is 1.0 when the orientation is completely random.

[0052] In this invention, the orientation parameter Os of the sheath component and the orientation parameter Oc of the core component of the core-sheath composite fiber in the non-fused portion of the spunbond nonwoven fabric are measured by the following method. In this invention, sea-island composite fibers are also included in core-sheath composite fibers, and in the case of sea-island composite fibers, as in the case of core-sheath composite fibers described above, when measuring and interpreting the orientation parameters Os and Oc, "sheath component" is read as "sea component" and "core component" is read as "island component" before performing the measurements. (1) A core-sheath type composite fiber is sampled from near the center of the non-fused area (approximately equidistant from the surrounding fused area), and the fiber sample is embedded in bisphenol epoxy resin. (2) After the resin has hardened, sections are cut using a microtome. The section thickness should be 2 μm. At this time, the section is cut at an angle from the fiber axis so that the cut surface is elliptical, and thereafter, measurements are taken at a point where the thickness of the minor axis of the ellipse is constant. Note that by keeping the cutting angle within 4°, the section can be considered parallel to the fiber axis within a 2 μm film thickness. (3) Line measurements of the Raman spectrum are performed by irradiating the fiber surface to the center of a section of the core-sheath type composite fiber in the non-fused portion with polarized light in the direction perpendicular to the fiber axis (parallel direction) and in the direction perpendicular to the fiber axis. (4) At the positions of the core component and sheath component of the core-sheath type composite fiber in the non-fused section, 810 cm in both the parallel and perpendicular directions. -1 Nearby and 840cm -1 Raman band intensity in the vicinity I 810 and I 840 Calculate the intensity ratio I 810 / I 840 Calculate. (5) The orientation parameter is calculated based on the following equation (a). If the core component is divided into multiple independent regions, the orientation parameter is measured in all regions and the highest value is adopted. Orientation parameter = (I 810 / I 840 ) 平行 / ( I 810 / I 840 ) 垂直 (a) (6) Perform the same measurement at three different locations along the fiber axis of the core-sheath composite fiber, calculate the average value of the orientation parameter, and round it to two decimal places.

[0053] If it is difficult to sample core-sheath type composite fibers near the center of the non-fused area (approximately equidistant from the surrounding fused areas), the measurement can also be performed using the following procedure. (1) The spunbond nonwoven fabric sample is embedded in bisphenol epoxy resin. (2) After the resin has hardened, a section is cut using a microtome so that the cut surface is near the center of the non-fused portion of the spunbond nonwoven fabric (approximately equidistant from the surrounding fused portion). The section thickness should be 2 μm. A section with a cutting angle of 4° or less from the fiber axis is selected for subsequent measurements. (3) Line measurements of the Raman spectrum are performed by irradiating the fiber surface to the center of a section of the core-sheath type composite fiber in the non-fused portion with polarized light in the direction perpendicular to the fiber axis (parallel direction) and in the direction perpendicular to the fiber axis. (4) At the positions of the core component and sheath component of the core-sheath type composite fiber in the non-fused section, 810 cm in both the parallel and perpendicular directions. -1 Nearby and 840cm -1 Raman band intensity in the vicinity I 810 and I 840 Calculate the intensity ratio I 810 / I 840 Calculate. (5) The orientation parameter is calculated based on the following equation (a). If the core component is divided into multiple independent regions, the orientation parameter is measured in all regions and the highest value is adopted. Orientation parameter = (I810 / I 840 ) 平行 / ( I 810 / I 840 ) 垂直 (a) (6) Perform the same measurements at three different non-fused sections of the spunbond nonwoven fabric, calculate the average value of the orientation parameter, and round it to two decimal places.

[0054] The basis weight of the spunbond nonwoven fabric of the present invention is 5 g / m². 2 More than 100g / m 2 The following is preferable: The basis weight of the spunbond nonwoven fabric is preferably 5 g / m². 2 Above, a comfortable 10g / m 2 More preferably 15 g / m² 2 As a result of the above, a spunbond nonwoven fabric with mechanical strength suitable for practical use is obtained. On the other hand, the basis weight of the spunbond nonwoven fabric is preferably 100 g / m². 2 More preferably 50g / m 2 More preferably 30 g / m 2 The following conditions result in a spunbond nonwoven fabric with appropriate flexibility suitable for practical use.

[0055] In this invention, the basis weight of the spunbond nonwoven fabric shall be determined in accordance with JIS L1913:2010 "General Nonwoven Fabric Testing Methods" "6.2 Mass per Unit Area", and the value obtained by the following procedure shall be adopted. (1) Take three 20cm x 25cm test pieces for every 1m of width of the sample. (2) Weigh the mass (g) of each under standard conditions. (3) The arithmetic mean is 1m 2 Mass per unit (g / m³) 2 It is expressed as ) and rounded to the first decimal place.

[0056] The thickness of the spunbond nonwoven fabric of the present invention is preferably 0.05 mm or more and 1.5 mm or less. A thickness of preferably 0.05 mm or more, more preferably 0.08 mm or more, and even more preferably 0.1 mm or more, or a thickness of preferably 1.5 mm or less, more preferably 1 mm or less, and even more preferably 0.8 mm or less, results in a spunbond nonwoven fabric that possesses flexibility and moderate cushioning properties, making it suitable for practical use.

[0057] In this invention, the thickness (mm) of the spunbond nonwoven fabric shall be the value measured in accordance with "5.1 Thickness" of JIS L1906:2000 "Test Method for General Long Fiber Nonwoven Fabrics".

[0058] Furthermore, the apparent density of the spunbond nonwoven fabric of the present invention is 0.05 g / cm³. 3 More than 0.30g / cm 3 Preferably, the apparent density of the spunbond nonwoven fabric is 0.30 g / cm³. 3 More preferably, 0.25 g / cm³ 3 More preferably, 0.20 g / cm³ 3 The following conditions allow for the development of a flexible texture without compromising the strength of the spunbond nonwoven fabric.

[0059] On the other hand, the apparent density of the spunbond nonwoven fabric is preferably 0.05 g / cm³. 3 More preferably, 0.08 g / cm³ 3 More preferably 0.10 g / cm³ 3 As a result of the above, the occurrence of fuzzing and delamination is suppressed, and a spunbond nonwoven fabric with sufficient strength for practical use is obtained.

[0060] In this invention, apparent density (g / cm³) 3 The value is calculated from the above-mentioned weight and thickness before rounding, based on the following formula, and rounded to the third decimal place. Apparent density (g / cm 3 )=[Balance (g / m 2 )] / [Thickness (mm)]×10 -3 .

[0061] The spunbond nonwoven fabric of the present invention has a longitudinal tensile strength per basis weight of 1.5 (N / 25mm) / (g / m²). 2 ) or more 3.0(N / 25mm) / (g / m 2 It is more preferable that the tensile strength per basis weight is 1.5 (N / 25mm) / (g / m). 2 ) or more, more preferably 1.6 (N / 25mm) / (g / m 2 ) or more preferably 1.7(N / 25mm) / (g / m 2 By having a strength of 3.0 (N / 25mm) / (g / m²) or higher, the spunbond nonwoven fabric will have sufficient strength for practical use. On the other hand, the transverse tensile strength per basis weight is preferably 3.0 (N / 25mm) / (g / m²). 2 By keeping the following conditions in place, it is possible to prevent a decrease in the flexibility of the spunbond nonwoven fabric or damage to its texture.

[0062] The longitudinal tensile strength per basis weight can be controlled by appropriately adjusting the MFR of the polypropylene resin, additives, average single fiber diameter, and / or the spinning rate described later, as well as the heat bonding conditions (shape of the bonded area, pressure ratio, temperature, and linear pressure, etc.).

[0063] The transverse tensile strength per basis weight of the spunbond nonwoven fabric of the present invention is 0.4 (N / 25mm) / (g / m²). 2 ) or more 2.0(N / 25mm) / (g / m 2 It is more preferable that the tensile strength per basis weight is 0.4 (N / 25mm) / (g / m). 2 ) or more, more preferably 0.6 (N / 25mm) / (g / m 2 ) or more, more preferably 0.8 (N / 25mm) / (g / m 2 By having a strength of 2.0 (N / 25mm) / (g / m²) or higher, the spunbond nonwoven fabric will have sufficient strength for practical use. On the other hand, the transverse tensile strength per basis weight is preferably 2.0 (N / 25mm) / (g / m²). 2 By keeping the following conditions in place, it is possible to prevent a decrease in the flexibility of the spunbond nonwoven fabric or damage to its texture.

[0064] The lateral tensile strength per unit weight can be controlled by appropriately adjusting the MFR of the polypropylene resin, additives, average single fiber diameter, and / or the spinning rate described later, as well as the heat bonding conditions (shape of the bonded area, pressure ratio, temperature, and linear pressure, etc.).

[0065] In this invention, the tensile strength per basis weight of the spunbond nonwoven fabric shall be determined in accordance with JIS L1913:2010 "General Test Methods for Nonwoven Fabrics," "6.3 Tensile Strength and Elongation (ISO Method)," and the value obtained by the following procedure shall be adopted. (1) Take three 25mm x 200mm test pieces for every 1m of nonwoven fabric width, with the longer side facing the longitudinal direction (longitudinal direction of the nonwoven fabric) and the transverse direction (width direction of the nonwoven fabric). (2) Grasp the test specimens and set them in the tensile testing machine at intervals of 200 mm. (3) A tensile test is performed at a tensile speed of 100 mm / min, and the maximum strength is measured. (4) Determine the average of the maximum strength measured for each test specimen, calculate the tensile strength per unit weight based on the following formula, and round to two decimal places. Tensile strength per unit area ((N / 25mm) / (g / m) 2 )) = [Average value of maximum strength (N / 25mm)] / Basis weight (g / m 2 ).

[0066] Furthermore, the lateral tensile strength per unit weight can be controlled by appropriately adjusting the MFR of the polypropylene resin, additives, average single fiber diameter, and / or the spinning speed and heat bonding conditions (shape of the bonded area, pressure ratio, temperature, and linear pressure, etc.) as described later.

[0067] The spunbond nonwoven fabric of the present invention possesses physical properties that allow it to withstand practical use even with a low basis weight, making it an environmentally friendly nonwoven fabric that can reduce the amount of plastic raw materials used. It can be widely used in sanitary materials, medical materials, daily necessities, and industrial materials. In particular, it can be suitably used as a base fabric for disposable diapers, sanitary products, and poultices in sanitary materials, and as protective clothing and surgical gowns in medical materials.

[0068] [Method for manufacturing spunbond nonwoven fabric] The present invention provides a method for producing a spunbond nonwoven fabric, which preferably comprises the steps of: spinning a polypropylene resin as a core component, having a branching index g of 0.950 or more and an isotactic pentad fraction (mmmm) of 0.950 or more and a sheath component, from a composite spinneret having an ejection port; cooling and solidifying the spun yarn; pulling and stretching it with an ejector at a spinning speed of 3500 m / min or more and 6500 m / min or less to obtain a core-sheath composite fiber; collecting the core-sheath composite fiber on a net to form a fiber web; and heat-bonding the fiber web. A preferred embodiment of the method for producing a spunbond nonwoven fabric of the present invention will be described in detail below.

[0069] (1) Process for obtaining core-sheath composite fibers The raw material resin used in the method for producing the spunbond nonwoven fabric of the present invention is a propylene-based resin in which the main repeating unit is propylene. Here, "main repeating unit" means that the repeating unit accounts for 90 mol% or more of the total resin. Therefore, specific examples of the raw material resin include a homopolymer of propylene, or a copolymer of propylene and various α-olefins. When a copolymer of propylene and various α-olefins is used as the raw material resin, the copolymerization ratio of the various α-olefins is preferably 10 mol% or less, more preferably 5 mol% or less, and even more preferably 3 mol% or less, from the viewpoint of increasing strength.

[0070] The core component raw resin used in this invention has a branching index g of 0.950 to 0.990 and an isotactic pentad fraction (mmmm) of 0.950 to 0.995 as determined by nuclear magnetic resonance spectroscopy. A branching index g of 0.950 or higher, preferably 0.965 or higher, and more preferably 0.980 or higher, prevents excessively high melt tension, ensures sufficient stretch-following ability during melt spinning, and allows for stable spinning. This is presumed to be because the inclusion of polypropylene with long-chain branches in the main chain skeleton promotes the entanglement of amorphous tie molecules penetrating microcrystals in the system during cooling and solidification (pseudo-crosslinking effect between microcrystals), and in the subsequent stretching process, the stretching stress is uniformly transmitted throughout the system (tendency toward uniform stretching), thereby reducing voids generated inside the fiber and suppressing yarn breakage. Furthermore, when the branching index g is 0.990 or less, crystallization progresses due to the microcrystal formation effect, and the sheet strength of the spunbond nonwoven fabric is improved by the increase in single-fiber strength.

[0071] The raw material resin for the core component used in this invention has an isotactic pentad fraction (mmmm) of 0.950 to 0.995 as determined by nuclear magnetic resonance spectroscopy. When the mesopentad fraction is 0.950 or higher, the high degree of crystallinity improves the yarn strength of the spunbond, resulting in a spunbond nonwoven fabric with mechanical strength suitable for practical use. When the mesopentad fraction is 0.995 or lower, the spinnability during melt spinning is maintained, and a stable spunbond nonwoven fabric can be obtained.

[0072] The raw material resin used in the present invention may be blended with other resin components, as long as the effects of the present invention are not impaired. Examples of other resin components include polyolefin resins such as polyethylene and poly-4-methyl-1-pentene, which have melting points close to those of polypropylene, as well as low-melting-point polyester resins and low-melting-point polyamide resins. From the viewpoint of imparting flexibility, low-crystallinity olefin resins are preferably used. For example, ethylene-propylene copolymers are suitably used as low-crystallinity olefin resins. The mass ratio of the other resin component is preferably 20% by mass or less, and more preferably 10% by mass or less, in order to fully express the properties of the polypropylene resin.

[0073] Furthermore, the raw material resin may be a so-called recycled resin that has been material-recycled. As the resin raw material for material recycling must have a melt flow rate that can be melt-spun by the spunbond method, a recycled raw material with the desired melt flow rate may be melted again and used, or if it does not have the desired melt flow rate, at least one radical generating agent from the group consisting of organic peroxides, azo compounds, and nitroxides may be added to the raw material resin to lower the molecular weight of the raw material resin and adjust the melt flow rate before use. It should be noted that using recycled resin is desirable because it can reduce the amount of virgin petrochemical raw materials used and reduce the environmental burden during the manufacture of spunbond nonwoven fabrics.

[0074] The aforementioned organic peroxides include ketone peroxides such as methyl ethyl ketone peroxide and methyl isobutyl ketone peroxide, diacyl peroxides such as dibenzoyl peroxide, di-(3,5,5-trimethylhexanoyl) peroxide, dilauroyl peroxide, didecanoyl peroxide, and di-(2,4-dichlorobenzoyl) peroxide, hydroperoxides such as t-butyl hydroperoxide, cumene hydroperoxide, diisopropylbenzene hydroperoxide, and 2,5-dimethylhexane-2,5-dihydroperoxide, di-t-butyl peroxide, dicumyl peroxide, 2,5-dimethyl-2,5-bis(t-butylperoxy)hexane, 2,5-dimethyl-2,5-bis(t-butylperoxy)hexine-3, and α,α'-bis(t-butylperoxy) Examples include dialkyl peroxides such as (-oxy)diisopropylbenzene, peroxyketals such as 1,1-bis(t-butylperoxy)-3,3,5-trimethylcyclohexane and 2,2-bis(t-butylperoxy)butane, alkyl peresters such as t-butylperoxyoctoate, t-butylperoxypivalate, t-butylperoxyneodecanoate, and t-butylperoxybenzoate, and peroxycarbonates such as di-(2-ethylhexyl)peroxydicarbonate, diisopropylperoxydicarbonate, bis(4-t-butylcyclohexyl)peroxydicarbonate, di-sec-butylperoxydicarbonate, and t-butylperoxyisopropyl carbonate. Among these, dialkyl peroxides are preferred because they allow for easy control of MFR.

[0075] Furthermore, examples of the aforementioned azo compounds include azobisisobutyronitrile and azobisisovaleronitrile.

[0076] Examples of nitroxides include sterically hindered hydroxylamine esters.

[0077] When directly melt-spinning the aforementioned raw material resin, methods using extruders such as single-screw or twin-screw extruders can be applied. The radical generating agent may be kneaded in an extruder and pelletized to form a polypropylene resin before being used for spinning, or the raw material resin and radical generating agent may be kneaded together during spinning using the extruder of the spinning machine, thereby obtaining the polypropylene resin simultaneously with melt spinning.

[0078] In the present invention, in order to set the branching index g to the range described above, in addition to the method of using the corresponding polypropylene resin for which the branching index g is described above, methods such as blending a branched polypropylene resin having a branched structure with a linear polypropylene resin, introducing a long-chain branched structure into the polypropylene molecule as described in Japanese Patent Publication No. 62-121704, or methods such as those described in Japanese Patent Publication No. 2869606 are preferably used, but among these, the method of blending a branched polypropylene resin with a linear polypropylene resin is preferred because the branching index g can be easily adjusted.

[0079] The amount of branched polypropylene resin added to the linear polypropylene resin is preferably 1% by mass or more and 20% by mass or less. By adding 1% by mass or more, more preferably 2% by mass or more, and even more preferably 3% by mass or more, crystal growth in the fibers can be inhibited, resulting in finer crystals. Furthermore, the reduced crystal orientation lowers the softening temperature of the fiber surface, allowing the fibers to fuse together firmly during the spunbond heat bonding process, resulting in a high-strength spunbond nonwoven fabric. On the other hand, by adding 20% ​​by mass or less, more preferably 15% by mass or less, and even more preferably 10% by mass or less, the yarn strength can be increased while maintaining the heat-adhesion properties of the spunbond without unnecessarily inhibiting crystal growth in the fibers.

[0080] Specific examples of the aforementioned branched-chain polypropylene resins include polypropylene manufactured by Basell (e.g., type names: "PF-814", "PF-633", "PF-611", "SD-632", etc.), polypropylene manufactured by Borealis (e.g., type name: "WB130HMS", etc.), and polypropylene manufactured by Dow (e.g., type names: "D114", "D201", "D206", etc.).

[0081] In this context, branched-chain polypropylene refers to polypropylene having five or fewer internally trisubstituted olefins per 10,000 carbon atoms. The presence of these internally trisubstituted olefins is 1 This can be confirmed by the proton ratio in the 1H-NMR spectrum.

[0082] The spinning temperature when melting and spinning polypropylene resin is preferably 200°C to 270°C. More preferably 210°C or higher, even more preferably 220°C or higher, even more preferably 260°C or lower, and even more preferably 250°C or lower. By setting the spinning temperature within the above range, a stable molten state can be achieved, and excellent spinning stability can be obtained.

[0083] The back pressure of the spinneret is preferably between 0.1 MPa and 6.0 MPa. By setting the back pressure to preferably 0.1 MPa or higher, more preferably 0.3 MPa or higher, and even more preferably 0.5 MPa or higher, it is possible to suppress deterioration of discharge uniformity and the occurrence of fiber diameter variations. On the other hand, by setting the back pressure to 6.0 MPa or lower, it is possible to prevent the spinneret from being enlarged in order to increase pressure resistance. The back pressure of the spinneret can be adjusted by the discharge hole diameter, discharge hole depth, spinning temperature, etc., with the discharge hole diameter having the greatest contribution.

[0084] Next, the spun filament is cooled. Methods for cooling the spun filament include, for example, forcibly blowing cold air onto the filament, allowing it to cool naturally with the ambient temperature around it, and adjusting the distance between the spinneret and the ejector, or a combination of these methods can be employed. The cooling conditions can be appropriately adjusted considering the discharge rate per single hole of the spinneret, the spinning temperature, and the ambient temperature.

[0085] The cooled and solidified yarn is pulled and stretched by compressed air injected from an ejector. The spinning speed is preferably 3500 m / min to 6500 m / min, more preferably 4000 m / min to 6500 m / min, and even more preferably 4500 m / min to 6500 m / min. By setting the spinning speed to 3500 m / min to 6500 m / min, high productivity is achieved, and the orientation and crystallization of the fibers are promoted, allowing for the production of high-strength long fibers. Normally, increasing the spinning speed deteriorates spinnability and makes it impossible to stably produce yarn, but by using a polypropylene resin with a specific MFR range, it is possible to stably spin the intended polypropylene fibers.

[0086] (2) Process of forming a fiber web Next, the resulting long fibers are collected on a moving net or similar surface to obtain a nonwoven fiber web. When the fibers are drawn at a high spinning speed, the fibers ejected from the ejector are collected on the net under controlled conditions by a high-speed airflow, making it easier to obtain a nonwoven fabric with less fiber entanglement and higher uniformity.

[0087] In this case, it is preferable that the spinning speed / line speed ratio be 18 or higher. By setting the spinning speed / line speed ratio to preferably 18 or higher, and more preferably 20 or higher, the fibers can be collected on the net as it moves with the fibers oriented in the longitudinal direction, and a nonwoven fabric with high strength in the longitudinal direction can be obtained.

[0088] Methods for uniformly aligning the direction of the fibers of the yarn ejected from the ejector include: a method of guiding the yarn by installing an angled plate between the ejector and the net; a method of separating the yarn into those that fall along the plate and those that fall along the grooves by providing grooves of different angles on the plate, thereby dispersing and opening the fibers in the direction of the nonwoven fiber web flow; and a method of arranging multiple plates of different angles in a comb-like manner at the ejector outlet, causing the yarn to fall along each plate to further disperse and open the fibers in the direction of the nonwoven fiber web flow.

[0089] In particular, a method of opening fibers by arranging multiple flat plates at different angles in a comb-like manner at the ejector outlet and allowing the yarn to fall along each plate is preferable for aligning the orientation of the fibers because it efficiently disperses fine fiber diameters in the direction of the nonwoven fiber web flow and allows for controlled opening with minimal deceleration.

[0090] (3) Heat bonding process A preferred embodiment is to temporarily bond the nonwoven fiber web, obtained by collecting fibers on a net, to one side of the net by contacting it with a hot flat roll. This prevents the surface layer of the nonwoven fiber web from peeling or being blown away during transport on the net, thereby preventing deterioration of the weave and improving transportability from fiber collection to heat bonding.

[0091] Then, the desired spunbond nonwoven fabric can be obtained by heat bonding the resulting nonwoven fiber web. The method for heat bonding the nonwoven fiber web is not particularly limited, but examples include using various rolls such as a heat embossing roll in which a pair of upper and lower roll surfaces are engraved (with raised and recessed areas), a heat embossing roll consisting of a combination of a roll with one flat (smooth) surface and a roll with an engraved (raised and recessed area) surface, and a heat calender roll consisting of a combination of an upper and lower pair of flat (smooth) rolls, or using ultrasonic vibration of a horn (ultrasonic bonding).

[0092] In particular, a preferred embodiment is a heat embossing roll in which a pair of upper and lower roll surfaces are engraved (with raised and recessed areas), or a combination of a roll with one roll surface being flat (smooth) and the other roll surface being engraved (with raised and recessed areas), because it offers excellent productivity, provides strength at partially adhesive areas, and maintains the texture and feel unique to nonwoven fabrics at non-adhesive areas.

[0093] As for the surface material of the heat embossing rolls, it is preferable to use a pair of metal rolls in order to obtain a sufficient heat-compression effect and to prevent the engraving (recessed portion) of one embossing roll from being transferred to the surface of the other roll.

[0094] The embossed bonding area ratio by the heat embossing roll is preferably 5% to 30%. By setting the bonding area to preferably 5% or more, more preferably 8% or more, and even more preferably 10% or more, a strength suitable for practical use as a spunbond nonwoven fabric can be obtained. On the other hand, by setting the bonding area to preferably 30% or less, more preferably 25% or less, and even more preferably 20% or less, a moderate flexibility suitable for practical use can be obtained. Even when ultrasonic bonding is used, it is preferable that the bonding area ratio be within the same range.

[0095] The term "adhesion area ratio" here refers to the proportion of the spunbond nonwoven fabric that is bonded. Specifically, when heat bonding is performed using a pair of rolls with protrusions and indentations, it refers to the proportion of the spunbond nonwoven fabric that is bonded to the portion where the protrusions of the upper roll and the lower roll overlap and contact the nonwoven fiber web. When heat bonding is performed using a roll with protrusions and a flat roll, it refers to the proportion of the spunbond nonwoven fabric that is bonded to the portion where the protrusions of the roll with protrusions contact the nonwoven fiber web. Furthermore, when ultrasonic bonding is performed, it refers to the proportion of the spunbond nonwoven fabric that is bonded to the portion that is heat-welded by ultrasonic processing.

[0096] The shape of the bonded area formed by thermal embossing or ultrasonic bonding is not particularly limited, but for example, circular, elliptical, square, rectangular, parallelogram, rhombus, regular hexagon, and regular octagon shapes can be used. Furthermore, it is preferable that the bonded area is uniformly located at regular intervals in both the longitudinal direction (conveying direction) and the width direction of the spunbond nonwoven fabric. By doing so, variations in the strength of the spunbond nonwoven fabric can be reduced.

[0097] In a preferred embodiment, the surface temperature of the heat embossing roll during heat bonding is set to a temperature between -50°C and -10°C lower (i.e., (Tm-50°C) to (Tm-10°C)) than the melting point of the polypropylene resin used (hereinafter sometimes referred to as Tm(°C)). By setting the surface temperature of the heat roll to preferably -50°C (i.e., Tm-50°C, the same applies hereinafter) or higher relative to the melting point of the polypropylene resin, and more preferably -45°C (Tm-45°C) or higher, a spunbond nonwoven fabric with appropriate heat bonding and strength suitable for practical use can be obtained. Furthermore, by setting the surface temperature of the heat embossing roll to preferably -10°C (Tm-10°C) or lower, and more preferably -15°C (Tm-15°C) or lower relative to the melting point of the polypropylene resin, excessive heat bonding can be suppressed, and appropriate flexibility for practical use can be obtained.

[0098] The linear pressure of the heat embossing roll during heat bonding is preferably 50 N / cm or more and 500 N / cm or less. By setting the linear pressure of the roll preferably to 50 N / cm or more, more preferably to 100 N / cm or more, and even more preferably to 150 N / cm or more, a spunbond nonwoven fabric with sufficient heat bonding and strength for practical use can be obtained. On the other hand, by setting the linear pressure of the heat embossing roll preferably to 500 N / cm or less, more preferably to 400 N / cm or less, and even more preferably to 300 N / cm or less, a suitable flexibility for practical use can be obtained.

[0099] Furthermore, to adjust the thickness of the spunbond nonwoven fabric, heat bonding can be performed using a thermal calender roll consisting of a pair of upper and lower flat rolls before and / or after heat bonding with the heat embossing roll described above. The pair of upper and lower flat rolls are metal rolls or elastic rolls with no irregularities on the surface of the rolls, and can be used in pairs of metal rolls or metal rolls and elastic rolls.

[0100] Furthermore, an elastic roll, in this context, refers to a roll made of a material that has elasticity compared to a metal roll. Examples of elastic rolls include so-called paper rolls such as paper, cotton, and aramid paper, as well as resin rolls made of urethane resin, epoxy resin, silicone resin, polyester resin, hard rubber, and mixtures thereof.

[0101] (4) Post-processing and other processes As described above, the spunbond nonwoven fabric of the present invention is a long-fiber nonwoven fabric manufactured by the spunbond method. The spunbond method offers excellent productivity and mechanical strength, and can suppress fluffing and fiber shedding that are common in short-fiber nonwoven fabrics. Furthermore, laminating the collected spunbond nonwoven fiber web or the heat-pressed spunbond nonwoven fabric (both denoted as S) in multiple layers with SS, SSS, and SSSS is a preferred embodiment because it improves productivity and uniformity of the fabric. It is also a preferred embodiment to use it laminated with other nonwoven fabrics.

[0102] Furthermore, in the method for producing spunbond nonwoven fabric of the present invention, a functional agent may be added to the obtained spunbond nonwoven fabric. Examples of functional agents include hydrophilic agents, water-repellent agents, oil-repellent agents, antistatic agents, antibacterial agents, antiviral agents, deodorants, fragrances, and cooling agents, but there are no particular limitations.

[0103] There are no particular limitations on the method of impregnation of the functional agent; impregnation, spraying, Kissroll, etc., can be used. [Examples]

[0104] Next, the spunbond nonwoven fabric of the present invention will be described in detail based on the examples. However, the present invention is not limited to these examples.

[0105] [Measurement method] The evaluation methods and measurement conditions used in the examples are described below. Unless otherwise specified, the measurements of each physical property were performed based on the methods described above.

[0106] (1) Melt flow rate of polypropylene resin (MFR, g / 10 min): The MFR of polypropylene resin was measured under conditions of a load of 2.16 kg and a temperature of 230°C.

[0107] (2) Branching index g(-) of polypropylene resin: The branching index g of polypropylene resins was determined using a Waters Alliance GPC / V2000 gel permeation chromatography (GPC) system equipped with a differential refractometer (RI) and a viscometer, and Waters Millennium GPC / CV analysis software. 32 Using 1,2,4-trichlorobenzene as the mobile phase solvent, with the antioxidant "Irganox 1076" manufactured by BASF Japan Ltd. added at a concentration of 0.5 mg / mL, and using "Novatec PP (registered trademark) FY6" manufactured by Nippon Polypropylene Co., Ltd. as the linear polypropylene resin, the sample injection volume (sample loop volume) was set to 0.2175 mL, and measurements were performed according to the method described above.

[0108] (3) Mesopentade fraction (mmmm)(-) of polypropylene resin: Dissolve the polypropylene resin sample in a solvent. 13The mesopentade fraction (mmmm) was determined using 1C-NMR under the following conditions. In addition to the aforementioned literature, the "New Edition Polymer Analysis Handbook" edited by the Japan Society for Analytical Chemistry, Polymer Analysis Research Group, Kinokuniya Shoten, January 1995, pp. 609-611, was consulted for the measurements. A. Measurement conditions • Equipment: Bruker DRX-500 ·Measurement nucleus: 13C nucleus (resonance frequency: 125.8MHz) ·Measurement concentration: 10% by mass • Solvent: Benzene / deuthorthodichlorobenzene = mass ratio 1:3 mixed solution ·Measurement temperature: 130℃ • Spin speed: 12Hz • NMR sample tube: 5mm tube • Pulse width: 45° (4.5μs) • Pulse repetition time: 10 seconds • Data points: 64K • Number of conversions: 10,000 • Measurement mode: complete decoupling B.Analysis conditions A Fourier transform was performed with a line broadening factor (LB) of 1.0, resulting in a mmmm peak of 21.86 ppm. Peak splitting was performed using WINFIT software (Bruker). During this process, the peak splitting was performed starting from the high-field side as follows, and then automatic peak fitting was performed using the accompanying software. After optimizing the peak splitting, the sum of the mmmm peak fractions was calculated. The above measurement was performed five times, and the average value was taken as the mesopentad fraction (mmmm) of this sample. ·peak (a)mrrm (b)mrrr (c)rrrr (d)rmrm (e)rmrr (f)mmrm (g)mmrr (h)rmmr (i)mmmr (j)mmmm.

[0109] (4) Spinning speed (m / min): Based on the average single fiber diameter and the solid density of the resin used, the average single fiber fineness (dtex) was calculated as the mass per 10,000 m of length, rounded to two decimal places. The spinning speed was calculated from the average single fiber fineness and the amount of resin extruded from each spinneret single hole (hereinafter abbreviated as single-hole extrusion rate) (g / min) set for each condition, based on the following formula. Spinning speed (m / min) = (10000 × [single-hole discharge rate (g / min)] / [average single fiber fineness (dtex)].

[0110] (5) Average fiber diameter (μm) of the core-sheath composite fibers constituting the spunbond nonwoven fabric: The measurement was performed using the VHX-D500 electronic device manufactured by Keyence Corporation, following the method described above.

[0111] (6) Orientation parameter of core component, orientation parameter of sheath component (-): The measurement was performed using the triple Raman spectrometer "T-64000" manufactured by Atago Bussan Co., Ltd., following the method described above. The measurement conditions were as follows. • Measurement mode: Micro-Raman (polarization measurement) Objective lens: ×100 • Beam diameter: 1 μm • Light source: Ar laser / 514.5nm • Laser power: 100mW (7) Melting peak temperature Tm (°C) of spunbond nonwoven fabric: The measurement device used was a Perkin-Elmer "DSC8500," and measurements were taken using the method described above. The measurement conditions were as follows: • In-device atmosphere: Nitrogen (20 mL / min) • Temperature and heat calibration: High-purity indium (Tm=156.61℃, ΔHm=28.70J / g) Temperature range: 20℃~200℃ • Heating rate: 20°C / min • Sample quantity: approximately 0.5-4 mg • Sample container: Standard aluminum container.

[0112] (8) Tensile strength per basis weight of spunbond nonwoven fabric ((N / 25mm) / (g / m) 2 )) The measuring device used was the "RTG-1250" manufactured by A&D Co., Ltd., and measurements were taken using the method described above.

[0113] [Example 1] (Polypropylene resin) For the core component, a linear polypropylene resin with an MFR of 200 g / 10 min, a branching index of 1.000 g, and a mesopentade fraction (mmmm) of 0.990 was used. Additionally, a branched polypropylene resin with an MFR of 4 g / 10 min, a branching index of 0.600, and a mesopentade fraction of 0.940 was used. These resins were mixed so that the linear polypropylene resin comprised 97% by mass and the branched polypropylene resin comprised 3% by mass, yielding a polypropylene resin with an MFR of 194 g / 10 min, a branching index of 0.988 g, a mesopentade fraction of 0.989, and a melting peak temperature (Tmc) of 160°C.

[0114] On the other hand, for the sheath component, a polypropylene resin with an MFR of 230 g / 10 min, a branching index of 1.000 g, a mesopentad fraction (mmmm) of 0.990, and a melting peak temperature (Tms) of 160 °C was used.

[0115] (Spunbond nonwoven fabric) The aforementioned polypropylene resin was fed into a single-screw extruder and melted at a spinning temperature of 240°C. From a rectangular die with a hole diameter of φ0.40 mm, the core-sheath ratio (core component (mass%): sheath component (mass%)) was 70:30, and the single-hole discharge rate was 0.40 g / min. After the obtained yarn was cooled and solidified, it was further stretched by pulling it using the pressure of compressed air sprayed from a rectangular ejector. The spinning speed at this time was 4100 m / min. Next, this was collected on a moving net to obtain a nonwoven fiber web. Subsequently, the obtained nonwoven fiber web was heat-bonded under conditions of a linear pressure of 500 N / cm and a heat bonding temperature of 140°C, resulting in a constituent fiber with an average single fiber diameter of 11.6 μm and a basis weight of 30 g / m².2 A spunbond nonwoven fabric was obtained. The heat embossing rolls used were a pair of upper and lower heat embossing rolls, with the upper roll being a metal embossing roll with a polka dot pattern engraved on it and an adhesive area ratio of 11%, and the lower roll being a metal flat roll. The tensile strength per basis weight in the longitudinal and transverse directions of the obtained spunbond nonwoven fabric was evaluated. The results are shown in Table 1.

[0116] [Example 2] In the spunbond nonwoven fabric, the process was the same as in Example 1, except that the core-sheath ratio (core component (mass%): sheath component (mass%)) was changed to 50:50. The average single fiber diameter of the constituent fibers was 11.6 μm and the basis weight was 30 g / m². 2 A spunbond nonwoven fabric was obtained. The tensile strength per unit weight in the longitudinal and transverse directions of the obtained spunbond nonwoven fabric was evaluated. The results are shown in Table 1.

[0117] [Example 3] In the case of (polypropylene resin), the mixing method was changed so that the core component of the polypropylene resin consisted of 92% by mass of linear polypropylene resin and 8% by mass of branched polypropylene resin, resulting in a polypropylene resin with an MFR of 184 g / 10 min, a branching index of 0.968, a mesopentade fraction of 0.986, and a melting point of 160°C. In the case of (spunbond nonwoven fabric), the procedure was the same as in Example 1 except that the spinning speed was changed to 4600 m / min, resulting in an average single fiber diameter of 11.0 μm and a basis weight of 30 g / m². 2 A spunbond nonwoven fabric was obtained. The tensile strength per unit weight in the longitudinal and transverse directions of the obtained spunbond nonwoven fabric was evaluated. The results are shown in Table 1.

[0118] [Example 4] In the spunbond nonwoven fabric, the process was the same as in Example 1, except that the spinning speed was changed to 3600 m / min. The average diameter of the constituent fibers was 12.5 μm, and the basis weight was 30 g / m². 2 A spunbond nonwoven fabric was obtained. The tensile strength per unit weight in the longitudinal and transverse directions of the obtained spunbond nonwoven fabric was evaluated. The results are shown in Table 1.

[0119] [Example 5] In the case of (polypropylene resin), the mixing method was changed so that the core component of the polypropylene resin consisted of 92% by mass of linear polypropylene resin and 8% by mass of branched polypropylene resin, resulting in a polypropylene resin with an MFR of 184 g / 10 min, a branching index g of 0.968, a mesopentade fraction of 0.986, and a melting point of 160°C. The polypropylene used for the sheath component of the polypropylene resin core component had an MFR of 230 g / 10 min, a branching index g of 1.000, a mesopentade fraction (mmmm) of 0.980, and a melting peak temperature of 150°C. In the case of (spunbond nonwoven fabric), the procedure was the same as in Example 1 except that the spinning speed was changed to 3800 m / min, resulting in an average single fiber diameter of 12.1 μm and a basis weight of 30 g / m². 2 A spunbond nonwoven fabric was obtained. The tensile strength per unit weight in the longitudinal and transverse directions of the obtained spunbond nonwoven fabric was evaluated. The results are shown in Table 1.

[0120] [Comparative Example 1] In the case of (polypropylene resin), a linear polypropylene resin with an MFR of 200 g / 10 min, a branching index of 1.000 g, and a mesopentade fraction (mmmm) of 0.940 was used, and the mixing was modified so that the linear polypropylene resin was 85% by mass and the branched polypropylene resin was 15% by mass, resulting in a polypropylene resin with an MFR of 171 g / 10 min, a branching index of 0.940 g, a mesopentade fraction of 0.940, and a melting point of 160°C. In the case of (spunbond nonwoven fabric), the process was the same as in Example 1 except that the spinning speed was changed to 3800 m / min, resulting in an average single fiber diameter of 12.1 μm and a basis weight of 30 g / m². 2 A spunbond nonwoven fabric was obtained. The tensile strength per unit weight in the longitudinal and transverse directions of the obtained spunbond nonwoven fabric was evaluated. The results are shown in Table 1.

[0121] [Comparative Example 2] In the case of (polypropylene resin), only polypropylene with an MFR of 200 g / 10 min, a branching index of 1.000 g, and a mesopentade fraction (mmmm) of 0.940 was used as the core component linear polypropylene resin, and branched polypropylene resin was not used. The process was the same as in Example 1, except that the average single fiber diameter of the constituent fibers was 11.6 μm and the basis weight was 30 g / m². 2 A spunbond nonwoven fabric was obtained. The tensile strength per unit weight in the longitudinal and transverse directions of the obtained spunbond nonwoven fabric was evaluated. The results are shown in Table 1.

[0122] [Table 1]

[0123] The spunbond nonwoven fabrics of Examples 1-5 have a branching index g of polypropylene resin of 0.950 to 0.990, and a tensile strength per basis weight of 1.5 ((N / 25mm) / (g / m) in the vertical direction. 2 )) or more, horizontal 0.4 ((N / 25mm) / (g / m 2 )) As described above, a high-strength spunbond nonwoven fabric was obtained.

[0124] On the other hand, the spunbond nonwoven fabric of Comparative Example 1, in which the branching index g of the polypropylene resin was less than 0.950, had high melt tension and insufficient stretch-following ability during melt spinning and stretching. Perhaps because the single filaments were not sufficiently stretched and solidified, the spunbond nonwoven fabric had low tensile strength per basis weight. Similarly, the spunbond nonwoven fabric of Comparative Example 2, in which the branching index g of the polypropylene resin was greater than 0.995, also had low tensile strength per basis weight. Perhaps because crystallization did not progress easily and the single filament strength was reduced.

[0125] Although the present invention has been described in detail using specific embodiments, it will be apparent to those skilled in the art that various modifications and variations are possible without departing from the intent and scope of the invention.

Claims

1. A spunbond nonwoven fabric composed of core-sheath composite fibers consisting of a core component and a sheath component, wherein the core component is a polypropylene resin having a branching index g of 0.950 or more and 0.990 or less and an isotactic pentad fraction (mmmm) of 0.950 or more and 0.995 or less, and the sheath component is a polypropylene resin, and the spunbond nonwoven fabric has fused portions and unfused portions.

2. The spunbond nonwoven fabric according to claim 1, wherein the orientation parameter Oc of the core component of the core-sheath type composite fiber in the non-fused portion is 5.0 or more and 8.0 or less.

3. The spunbond nonwoven fabric according to claim 1 or 2, wherein the ratio Oc / Os of the orientation parameter of the core component to the orientation parameter Os of the sheath component of the core-sheath composite fiber in the non-fused portion is 1.2 or more and 2.0 or less.

4. The spunbond nonwoven fabric according to claim 1 or 2, wherein the melting peak temperature Tms (°C) of the sheath component and the melting peak temperature Tmc (°C) of the core component of the core-sheath composite fiber satisfy the following formula 1. Tmc-30≦Tms≦Tmc-5 (Formula 1)

5. The process involves spinning a polypropylene resin as the core component, having a branching index g of 0.950 or more and an isotactic pentad fraction (mmmm) of 0.950 or more and a sheath component of polypropylene resin, from a composite spinneret having an ejection port, then cooling and solidifying the spun yarn, and then pulling and stretching it with an ejector at a spinning speed of 3500 m / min or more and 6500 m / min or less to obtain a core-sheath composite fiber. The process involves collecting the core-sheath composite fibers onto a net to form a fiber web, The process of heat-bonding the aforementioned fiber web, A method for producing a spunbond nonwoven fabric having [the specified characteristics].

Citation Information

Patent Citations

  • Heat-fusible conjugated fiber and nonwoven fabric using the same

    JP1996074128A

  • Preparation of fiber for high strength non-woven material and obtained fiber and non-woven material

    JP1996246228A

  • Polypropylene-based nonwoven fabric

    JP2000064168A

  • Polypropylene fibers and products made from them

    JP2000507654A

  • Spun-bonded nonwoven fabric and absorbing article

    JP2002069820A