Laminated film and method for manufacturing the same
A laminated film with a polypropylene base, intermediate, and heat seal layer structure addresses low-temperature sealing and strength issues, achieving high heat seal strength, low-temperature sealability, and recyclability for heavy-duty packaging with reduced resin use.
Patent Information
- Application Number
- JP2026028434
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2026-02-25
- Publication Date
- 2026-11-11
- Estimated Expiration
- 2045-10-27
AI Technical Summary
Existing laminated films made of polypropylene are inferior in low-temperature heat sealing, heat seal strength, impact resistance, puncture strength, and tear strength, limiting their applications and recyclability.
A laminated film structure comprising a stretched polypropylene base layer, an intermediate polypropylene layer, and an unstretched polypropylene heat seal layer, with specific resin compositions for each layer that enhance heat seal strength, low-temperature sealability, and recyclability.
The laminated film achieves high heat seal strength, low-temperature sealability, and recyclability, enabling applications in heavy-duty packaging while reducing resin use and energy consumption, and is composed of polypropylene monomaterials for improved environmental compliance.
Smart Images

Figure 0007948469000003 
Figure 0007948469000001 
Figure 0007948469000002
Abstract
Description
[Technical Field]
[0001] The present invention relates to a laminated film with excellent seal strength and low-temperature sealability, and a method for manufacturing the same. [Background technology]
[0002] Polypropylene film possesses various excellent properties such as transparency, rigidity, and heat resistance, and is therefore widely used as packaging film for food, clothing, medical supplies, pharmaceuticals, stationery, general merchandise, industrial materials, and industrial applications. In particular, films made by dry laminating biaxially oriented polyamide film, biaxially oriented polyester film, biaxially oriented polypropylene film, etc., with polyethylene are mainstream in the market and are used for food packaging and as outer casing material for lithium-ion batteries. On the other hand, in recent years, due to growing awareness of environmental issues, there has been increasing interest in so-called monomaterial packaging materials that use the same material for packaging and have recyclability. Although polypropylene film has the advantage of a higher melting point and rigidity compared to polyethylene film, its applications are limited because it is inferior in heat seal strength, low-temperature heat sealability, impact resistance, puncture strength, and tear strength, and has poor resistance to bag drop at low temperatures.
[0003] For example, Patent Document 1 discloses a retort sealant film comprising a core layer consisting of 0 to 150 parts by weight of polypropylene resin per 100 parts by weight of polypropylene elastomer, and a heat seal layer laminated on at least one side of the core layer, which consists of a mixture of 30 to 70 parts by weight of polypropylene resin and 70 to 30 parts by weight of polypropylene elastomer, and it is shown to have excellent impact resistance and low-temperature sealing properties.
[0004] Patent documents 2 and 3 disclose a packaging material comprising at least a biaxially oriented polypropylene film and a polypropylene-based unoriented film, wherein the polypropylene-based unoriented film contains a propylene homopolymer and a propylene-ethylene random copolymer, and it is shown that the balance between heat resistance and low-temperature sealing performance can be improved.
[0005] On the other hand, laminated films are also known in which three or more layers, including a layer made of polypropylene resin, are laminated. Patent Document 4 discloses a laminated structure comprising a gas barrier laminated film having a gas barrier layer made of a stretched polypropylene resin substrate and an inorganic thin film, and a sealant film, and it is shown that it is made of a resin species with low environmental impact and has the necessary performance such as gas barrier properties and heat sealability. Patent Document 5 discloses a laminated structure comprising a sealant film and a substrate film that meet specific requirements, wherein the sealant film has a heat-sealable layer and an adjacent layer, and when the total mass of the two types of films is 100% by mass, it contains 70% by mass or more of propylene(co)polymer and / or 1-butene(co)polymer, and it is shown that it has a high content of propylene copolymer and excellent low-temperature heat sealability and heat seal strength. [Prior art documents] [Patent Documents]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 9-150491 [Patent Document 2] Japanese Patent Publication No. 2023-161216 [Patent Document 3] Japanese Patent Publication No. 2023-161210 [Patent Document 4] International Publication No. 2025 / 070687 [Patent Document 5] Japanese Patent Publication No. 2020-192696 [Overview of the project] [Problems that the invention aims to solve]
[0007] The sealant film described in Patent Document 1, the packaging materials described in Patent Documents 2 and 3, and the laminate described in Patent Document 4 were inferior in low-temperature heat sealing, and there was room for improvement in heat seal strength. In the laminate described in Patent Document 5, low-temperature heat sealing was good, but there was room for improvement in heat seal strength.
[0008] The object of the present invention is to provide a laminated film with excellent heat seal strength, low-temperature sealability, and recyclability. [Means for solving the problem]
[0009] As a result of diligent research to solve the above problems, the inventors have found that in a laminated film in which a base layer, an intermediate layer, and a heat seal layer are laminated in this order, the base layer and intermediate layer are stretched polypropylene films, the heat seal layer is an unstretched polypropylene film, and the resin compositions constituting the intermediate layer and the heat seal layer each satisfy specific requirements, the resulting laminated film exhibits excellent heat seal strength, low-temperature sealability, and recyclability, thus completing the present invention. The present invention relates to the following [1] to
[10] .
[0010] [1] A laminated film comprising a base layer, an intermediate layer, and a heat seal layer in this order, wherein the base layer and the intermediate layer are stretched polypropylene films, the heat seal layer is an unstretched polypropylene film, the resin composition (A) constituting the intermediate layer satisfies the following requirement (a1), and the resin composition (B) constituting the heat seal layer satisfies the following requirements (b1) and (b2). (a1) The durometer D hardness (HDD) measured in accordance with JIS K 7215:1986 is 10 to 78. (b1) The durometer D hardness (HDD) measured in accordance with JIS K 7215:1986 is 10 to 78. (b2) Its melting point is 110-150°C. [2] The resin composition (A) comprises a propylene polymer (C) and a propylene thermoplastic elastomer (D), wherein the content of the propylene polymer (C) is 10 to 100% by weight and the content of the propylene thermoplastic elastomer (D) is 0 to 90% by weight, based on 100% by weight of the total of the propylene polymer (C) and the propylene thermoplastic elastomer (D). The resin composition (B) comprises a propylene polymer (E) and a propylene thermoplastic elastomer (F), wherein the content of the propylene polymer (E) is 10 to 100% by weight and the content of the propylene thermoplastic elastomer (F) is 0 to 90% by weight, based on a total weight of 100% by weight of the propylene polymer (E) and the propylene thermoplastic elastomer (F). The laminated film according to [1], wherein the propylene polymer (C) satisfies the following requirements (c1) to (c5), the propylene thermoplastic elastomer (D) satisfies the following requirements (d1) to (d4), the propylene polymer (E) satisfies the following requirements (e1) to (e5), and the propylene thermoplastic elastomer (F) satisfies the following requirements (f1) to (f4). (c1) and (e1) The MFR measured in accordance with JIS K 7210-1:2014 (230℃, 2.16kg load) is 1 to 50g / 10min. (c2) and (e2) In accordance with JIS K 7171:2022, the flexural modulus measured at a test speed of 2 mm / min is greater than 500 MPa and less than or equal to 1,300 MPa. The content of units derived from (c3) and (e3) propylene exceeds 88.0% by weight and is 99.9% by weight or less. (c4) and (e4) contain units derived from ethylene and α-olefins having 4 to 20 carbon atoms in a quantity of 0.1% by weight or more and less than 12.0% by weight. (c5) and (e5) have melting points of 110-155°C. (d1) and (f1) The MFR measured in accordance with JIS K 7210-1:2014 (230℃, 2.16kg load) is 1 to 30g / 10min. (d2) and (f2) The flexural modulus measured at a test speed of 2 mm / min in accordance with JIS K 7171:2022 is 5 to 200 MPa. (d3) and (f3) The content of units derived from propylene is 60.0 to 92.0% by weight. (d4) and (f4) The content of units derived from ethylene and α-olefins having 4 to 20 carbon atoms is 8.0 to 40.0% by weight. [3] The laminated film according to [2], wherein the propylene-based thermoplastic elastomer (D) satisfies the following requirements (d3') and (d4'), and the propylene-based thermoplastic elastomer (F) satisfies the following requirements (f3') and (f4'). (d3') and (f3') The content of units derived from propylene is 60.0 to 88.0% by weight. (d4') and (f4') The content of units derived from ethylene and α-olefins having 4 to 20 carbon atoms is 12.0 to 40.0% by weight. [4] The laminated film according to [2] or [3], wherein in the resin composition (B), the content of the propylene-based polymer (E) is 50 to 95% by weight and the content of the propylene-based thermoplastic elastomer (F) is 5 to 50% by weight, based on 100% by weight of the total of the propylene-based polymer (E) and the propylene-based thermoplastic elastomer (F). [5] The laminated film according to any one of [1] to [4], wherein the thicknesses of the intermediate layer and the heat seal layer are 1 to 10 μm and 10 to 400 μm, respectively. [6] The laminated film according to any one of [1] to [5], wherein the sealing temperature at which the heat seal strength reaches 20 N / 15 mm, measured under the following conditions, is 140°C or lower. <Measurement of sealing temperature at which heat seal strength reaches 20 N / 15 mm> After storing the laminated film at an ambient temperature of 23°C for 7 days, it is cut into strips of 180 mm (MD) × 80 mm (TD), folded in half along the MD direction so that the heat seal layers are in contact with each other, and heat-sealed at a position 20 to 30 mm from the fold line with a width of 10 mm under the following sealing conditions. The obtained partially heat-sealed sample is cut into strips so that the TD has a width of 15 mm to obtain a test piece. For the obtained test piece, both ends of the test piece are pulled in a 180° peeling direction at a speed of 500 mm / min using a Schopper-type tensile tester, and the maximum value of the force required to peel off the heat-sealed part is measured and defined as the heat seal strength. The sealing conditions are: sealing pressure: 2.0 kg / cm 2 (0.196 MPa), sealing time: 1.0 second, and sealing temperature: in the range of 90°C to 170°C, in increments of 10°C. In the sealing curve obtained from the sealing temperature and the heat seal strength, the data between any two points measured at every 10°C of sealing temperature is approximated by a linear function, and the sealing temperature at which the heat seal strength reaches 20 N / 15 mm is determined. [7] The laminated film according to any one of [1] to [6], wherein in a bag drop impact test measured under the following conditions, the average value of the number of bag breakage drops is 6 or more. <Bag Drop Impact Test> Two sheets of 120 mm × 150 mm are cut from the laminated film, the heat seal layers of the respective sheets are superposed on each other, and then three sides are sealed with an impulse sealer under the following sealing conditions to prepare a 120 mm × 150 mm sample bag. 100 ml of water is poured into the sample bag, and the unsealed one side is sealed with an impulse sealer under the following sealing conditions to prepare a water-sealed test piece. After the water-sealed test piece is stored in an atmosphere of 0°C for 1 day, it is dropped 50 times continuously from a height of 1.5 m onto a metal plate, and the maximum number of times without bag breakage is defined as the number of bag breakage drops. The test is repeated 5 times, and the average value of the number of bag breakage drops is determined. The sealing conditions are as follows: using a poly sealer manufactured by Fuji Impulse Co., Ltd. (trade name: PC-300), the sealing width is 2 mm, and the scale is 10 (sealing time 1.6 seconds). A food packaging film, a heavy goods packaging film, or a liquid packaging film made of a laminated film as described in any one of [8][1] to [7]. [9] A method for manufacturing a laminated film according to any one of [1] to [7], comprising: step 1 of co-extruding a base layer and an intermediate layer to obtain a laminate; step 2 of stretching the laminate obtained in step 1 to obtain a stretched film; and step 3 of adhering a heat seal layer onto the intermediate layer of the stretched film obtained in step 2.
[10] The method for manufacturing a laminated film according to [9], wherein step 3 is a step of bonding the intermediate layer and the heat seal layer by a dry lamination method. [Effects of the Invention]
[0011] The present invention provides a laminated film with excellent heat seal strength, low-temperature sealability, and recyclability. [Brief explanation of the drawing]
[0012] [Figure 1] Figure 1 is a schematic diagram showing the process flow when using one horizontal polymerizer in the production of propylene-based polymers-1 and 2 according to the present invention. [Modes for carrying out the invention]
[0013] The laminated film is formed by laminating a base layer, an intermediate layer, and a heat-seal layer in this order, the base layer and the intermediate layer being stretched polypropylene films, and the heat-seal layer being an unstretched polypropylene film. The resin composition (A) constituting the intermediate layer satisfies the following requirement (a1), and the resin composition (B) constituting the heat-seal layer satisfies the following requirements (b1) and (b2). (a1) The durometer D hardness (HDD) measured in accordance with JIS K 7215:1986 is 10 to 78. (b1) The durometer D hardness (HDD) measured in accordance with JIS K 7215:1986 is 10 to 78. (b2) Its melting point is 110-150°C. By laminating the base layer, intermediate layer, and heat seal layer of the present invention in this order, a laminated film with excellent heat seal strength, low-temperature sealability, and recyclability can be obtained. The inventors have found that a laminated film with an intermediate layer that meets specific requirements between the base layer and the heat seal layer exhibits significantly improved heat seal strength compared to a conventional laminated film without an intermediate layer. This intermediate layer is flexible and is thought to effectively distribute the stress generated when peeling the laminated film after heat sealing. As a result, it is possible to prevent stress from concentrating in the base layer and suppress the occurrence of cracks in the base layer and the resulting fracture of the base layer. This is presumed to improve the overall heat seal strength of the laminated film. The laminated film of the present invention achieves high heat seal strength, enabling its application in heavy-duty packaging, which was not possible with conventional polypropylene laminated films. Furthermore, in light of recent market demands for environmental compliance, there is a need to reduce the amount of resin used in the film sector. The laminated film achieves high heat seal strength even with a thin heat seal layer, allowing for a thinner heat seal layer than conventional films and thus reducing the amount of resin used. In addition, the heat seal initiation temperature can be lowered, allowing for a reduction in the set temperature of the sealing mold, thus contributing to energy savings. Furthermore, since the base layer, intermediate layer, and heat-seal layer of the present invention are all polypropylene monomaterial films, they have excellent recyclability, particularly in terms of material recyclability. In this specification, a polypropylene monomaterial film means a film in which almost all of the raw materials constituting the film are composed of polypropylene, and more specifically, a film in which all the resins constituting the film are polymers containing 50% by weight or more polymerization units derived from propylene. In this specification, a polypropylene film means a film in which all the resins constituting the film are polymers containing 50% by weight or more polymerization units derived from propylene. In polypropylene monomaterial films and polypropylene films, the content ratio of polymerization units derived from propylene to 100% by weight of all resins constituting the film is preferably 50% by weight or more, and more preferably 60% by weight or more.
[0014] In this specification, the base layer, intermediate layer, and heat seal layer, as well as the resin compositions (A) and (B), and the propylene polymer (C), propylene thermoplastic elastomer (D), propylene polymer (E), and propylene thermoplastic elastomer (F) are each polymers containing 50% by weight or more of polymerization units derived from propylene. The following describes each component, its manufacturing method, and its applications.
[0015] <Middle class> The intermediate layer is a stretched polypropylene film, and the resin composition (A) constituting the intermediate layer satisfies the following requirement (a1). By satisfying the following requirement (a1) of the resin composition (A), the intermediate layer can disperse the stress generated in the laminated film during heat seal strength measurement. As a result, cracking and fracture of the base layer can be suppressed, and the heat seal strength can be improved. (a1) The durometer D hardness (HDD) measured in accordance with JIS K 7215:1986 is 10 to 78.
[0016] <<Resin composition (A)>> The resin composition (A) satisfies the following requirement (a1). (a1) The durometer D hardness (HDD) measured in accordance with JIS K 7215:1986 is 10 to 78. From the viewpoint of improving the heat seal strength of the laminated film, the durometer D hardness (HDD) of the resin composition (A) is preferably 10 to 78, more preferably 20 to 75, and more preferably 30 to 70.
[0017] The resin composition (A) preferably further satisfies the following requirements (a2) to (a6).
[0018] (a2) Its melting point is 110-150°C. From the viewpoint of the flexibility of the intermediate layer, the melting point of the resin composition (A) is preferably 110 to 150°C, and more preferably 110 to 140°C.
[0019] In this specification, the method for measuring the melting point and the heat of fusion ΔHm is as follows: Using a differential scanning calorimeter (DSC), a sample of 5.0 mg is heated to 200°C, held at 200°C for 5 minutes, and then the temperature is lowered to 40°C at a rate of 10°C / min. Next, when the sample is heated at a rate of 10°C / min, the top temperature of the endothermic peak is defined as the melting peak temperature (melting point / Tm), and the peak area of this peak is defined as ΔHm (J / g).
[0020] (a3) The flexural modulus measured at a test speed of 2 mm / min in accordance with JIS K 7171:2022 is 10 to 1,300 MPa. From the viewpoint of improving the heat seal strength of the laminated film, the flexural modulus of the resin composition (A) is preferably 10 to 1,300 MPa, more preferably 100 to 1,200 MPa, even more preferably 200 to 1,100 MPa, and particularly preferably 300 to 1,000 MPa.
[0021] (a4) In accordance with JIS K 7127:1999, the Young's modulus in the flow direction (MD) measured at a tensile speed of 1 mm / min is 10 to 700 MPa. From the viewpoint of improving the heat seal strength of the laminated film, the Young's modulus of the resin composition (A) is preferably 10 to 700 MPa, more preferably 100 to 650 MPa, and even more preferably 200 to 600 MPa.
[0022] (a5) The heat of fusion ΔHm is 5 to 100 J / g. From the viewpoint of improving the heat seal strength of the laminated film, the heat of fusion ΔHm of the resin composition (A) is preferably 5 to 100 J / g, more preferably 10 to 95 J / g, and even more preferably 20 to 90 J / g.
[0023] (a6) Density measured at 23°C in accordance with JIS K 7112-2:2023 is 0.850~0.899 g / cm³ 3 That is the case. From the viewpoint of improving the heat seal strength of the laminated film, the density of the resin composition (A) is 0.850 to 0.899 g / cm³. 3 Preferably, it is 0.860 to 0.898 g / cm³. 3 It is more preferable that the value be 0.870-0.897 g / cm³. 3 It is even more preferable that this be the case.
[0024] From the viewpoint of improving heat seal strength, the resin composition (A) contains a propylene polymer (C) and optionally a propylene thermoplastic elastomer (D). Preferably, the content of the propylene polymer (C) is 10 to 100% by weight and the content of the propylene thermoplastic elastomer (D) is 0 to 90% by weight, based on 100% by weight of the total of the propylene polymer (C) and the propylene thermoplastic elastomer (D). More preferably, the content of component (C) relative to 100% by weight of the total of component (C) and component (D) is 40 to 90% by weight, even more preferably 50 to 85% by weight, and particularly preferably 60 to 80% by weight. Similarly, the content of component (D) relative to 100% by weight of the total of component (C) and component (D) is 10 to 60% by weight, even more preferably 15 to 50% by weight, and particularly preferably 20 to 40% by weight.
[0025] <<<Propylene-based polymer (C)>>> The propylene polymer (C) is a copolymer of propylene and ethylene or an α-olefin having 4 to 20 carbon atoms in a content of 0.1% by weight or more, and preferably satisfies the following requirements (c1) to (c5). The copolymer components with propylene, ethylene and α-olefins having 4 to 20 carbon atoms, may be one type or a combination of two or more types. The copolymer components are preferably ethylene or α-olefins having 4 to 10 carbon atoms. Specifically, examples of copolymer components include ethylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-decene, 3-methyl-1-butene, 4-methyl-1-pentene, 2-methyl-1-pentene, 2-methyl-1-hexene, etc., with ethylene or 1-butene being particularly preferred. The propylene polymer (C) may also be a blend of two or more types of polymers: a propylene homopolymer and a random copolymer of propylene and ethylene or an α-olefin having 4 to 20 carbon atoms. The blend may be a melt blend obtained by melt-kneading these polymers that have been manufactured separately, or a polymer blend obtained as a multi-stage polymer produced by the multi-stage polymerization method described later. The propylene polymer (C) may be used alone or in combination of two or more types.
[0026] In this specification, the percentage of units derived from ethylene in a propylene-ethylene copolymer is a value calculated based on the following formula. Percentage of units derived from ethylene (%) = Weight of units derived from ethylene / (Weight of units derived from propylene + weight of units derived from ethylene) × 100 The proportion of units derived from each monomer in other copolymers, such as propylene-ethylene-1-butene copolymer, can also be calculated in the same manner as described above.
[0027] (c1) The MFR measured in accordance with JIS K 7210-1:2014 (230℃, 2.16kg load) is 1 to 50g / 10min. The propylene polymer (C) preferably has a melt flow rate (MFR) of 1 to 50 g / 10 min, measured in accordance with JIS K 7210-1:2014 (230°C, 2.16 kg load). More preferably, the MFR is 2 to 40 g / 10 min, and even more preferably 3 to 30 g / 10 min. Having an MFR of 1 to 50 g / 10 min for the propylene polymer (C) results in good compatibility with the propylene thermoplastic elastomer (D) and good film processability. Methods for controlling the MFR value are well known, and it can be easily adjusted by adjusting the temperature and pressure, which are polymerization conditions for the propylene polymer (C), or by controlling the amount of chain transfer agent such as hydrogen added during polymerization.
[0028] (c2) In accordance with JIS K 7171:2022, the flexural modulus measured at a test speed of 2 mm / min is greater than 500 MPa and less than or equal to 1,300 MPa. The propylene polymer (C) preferably has a flexural modulus of elasticity exceeding 500 MPa and 1,300 MPa or less, as measured at a test speed of 2 mm / min in accordance with JIS K 7171:2022. More preferably, the upper limit of the flexural modulus is 1,200 MPa or less, and even more preferably 1,000 MPa or less. By setting the flexural modulus within the above range, the flexibility of the intermediate layer can be maintained and the heat seal strength can be improved. Methods for controlling the flexural modulus are well known, and it can be easily adjusted by controlling the content ratio of copolymerized ethylene and / or α-olefins having 4 to 20 carbon atoms.
[0029] (c3) The content of units derived from propylene exceeds 88.0% by weight and is 99.9% by weight or less. The content of propylene-derived units in the propylene polymer (C) is preferably greater than 88.0% by weight and 99.9% by weight or less. By keeping the content of propylene-derived units within the above range, the flexibility of the intermediate layer can be maintained. The content of propylene-derived units is more preferably greater than 88.5% by weight and 98.0% by weight, and even more preferably greater than 89.0% by weight and 97.0% by weight.
[0030] (c4) The content of units derived from ethylene and α-olefins having 4 to 20 carbon atoms is 0.1% by weight or more and less than 12.0% by weight. The content of units derived from ethylene and α-olefins having 4 to 20 carbon atoms in the propylene polymer (C) is preferably 0.1% by weight or more and less than 12.0% by weight. By keeping the content of units derived from ethylene and α-olefins having 4 to 20 carbon atoms within the above range, the flexibility of the intermediate layer can be maintained. The content of units derived from ethylene and α-olefins having 4 to 20 carbon atoms is more preferably 2.0% by weight to less than 11.5% by weight, and even more preferably 3.0% by weight to less than 11.0% by weight. The content of ethylene-derived units in the propylene polymer (C) is preferably 0.1 to 7.0% by weight, and more preferably 1.0 to 5.0% by weight. The content of units derived from 1-butene in the propylene polymer (C) is preferably 0 to 11.0% by weight, and more preferably 0 to 10.0% by weight. The total content of units derived from ethylene and 1-butene in the propylene polymer (C) is preferably 0.1% by weight or more and less than 12.0% by weight, more preferably 2.0% to less than 11.5% by weight, and even more preferably 3.0% to less than 11.0% by weight.
[0031] (c5) The melting point is 110-155°C. The melting point of the propylene polymer (C) is preferably 110 to 155°C, more preferably 115 to 145°C, and even more preferably 120 to 140°C. By setting the melting point in the range of 110 to 155°C, good heat seal strength and low-temperature sealability can be achieved. Methods for controlling the melting point are well known, and it can be easily adjusted by controlling the content ratio of copolymerized ethylene and / or α-olefins having 4 to 20 carbon atoms.
[0032] From the viewpoint of imparting flexibility to the intermediate layer, the propylene polymer (C) is preferably a propylene-ethylene copolymer or a propylene-ethylene-1-butene copolymer that satisfies the above requirements (c1) to (c5), and more preferably a propylene-ethylene-1-butene copolymer.
[0033] <<<Propylene-based thermoplastic elastomer (D)>>> The propylene-based thermoplastic elastomer (D) is a copolymer of propylene and ethylene or an α-olefin having 4 to 20 carbon atoms, and preferably satisfies the following requirements (d1) to (d4). The copolymer components with propylene, ethylene and α-olefins having 4 to 20 carbon atoms, may be one type or a combination of two or more types. The copolymer components are preferably ethylene or α-olefins having 4 to 10 carbon atoms. Specifically, examples of copolymer components include ethylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-decene, 3-methyl-1-butene, 4-methyl-1-pentene, 2-methyl-1-pentene, 2-methyl-1-hexene, etc., with ethylene or 1-butene being particularly preferred. Examples of propylene-based thermoplastic elastomers (D) include random copolymer rubbers of propylene and ethylene or α-olefins having 4 to 20 carbon atoms, specifically propylene-ethylene copolymers and propylene-ethylene-1-butene copolymers. The propylene-based thermoplastic elastomer (D) may be used alone or in combination of two or more types.
[0034] (d1) The MFR measured in accordance with JIS K 7210-1:2014 (230℃, 2.16kg load) is 1 to 30g / 10min. The propylene-based thermoplastic elastomer (D) preferably has an MFR of 1 to 30 g / 10 min, measured in accordance with JIS K 7210-1:2014 (230°C, 2.16 kg load). More preferably, the MFR is 2 to 20 g / 10 min, and even more preferably 2 to 10 g / 10 min. When the MFR of the propylene-based thermoplastic elastomer (D) is within the range of 1 to 30 g / 10 min, a film with good moldability and appearance can be obtained. Methods for controlling the MFR value are well known, and it can be easily adjusted by controlling the temperature and pressure, which are polymerization conditions for propylene-based thermoplastic elastomers (D), or by controlling the amount of chain transfer agents such as hydrogen added during polymerization.
[0035] (d2) The flexural modulus measured at a test speed of 2 mm / min in accordance with JIS K 7171:2022 is 5 to 200 MPa. The propylene-based thermoplastic elastomer (D) preferably has a flexural modulus of 5 to 200 MPa, measured at a test speed of 2 mm / min in accordance with JIS K 7171:2022. More preferably, the flexural modulus is 5 to 150 MPa, and even more preferably 5 to 100 MPa. When the flexural modulus is within the above range, the flexibility of the intermediate layer is improved, and the heat seal strength and resistance to bag drop are improved. Methods for controlling the flexural modulus are well known, and it can be easily adjusted by controlling the content ratio of copolymerized ethylene and / or α-olefins having 4 to 20 carbon atoms.
[0036] (d3) The content of units derived from propylene is 60.0 to 92.0% by weight. The content of propylene-derived units in the propylene-based thermoplastic elastomer (D) is preferably 60.0 to 92.0% by weight. By setting the content of propylene-derived units within the above range, the flexibility of the intermediate layer can be improved and the heat seal strength can be improved. The content of propylene-derived units is more preferably 60.0 to 88.0% by weight, even more preferably 60.0 to 87.0% by weight, and particularly preferably 64.0 to 85.0% by weight.
[0037] (d3) can also be expressed as (d3') below. The content of units derived from (d3')propylene is 60.0 to 88.0% by weight.
[0038] (d4) The content of units derived from ethylene and α-olefins having 4 to 20 carbon atoms is 8.0 to 40.0% by weight. The content of units derived from ethylene and α-olefins having 4 to 20 carbon atoms in the propylene-based thermoplastic elastomer (D) is preferably 8.0 to 40.0% by weight. By setting the content of units derived from ethylene and α-olefins having 4 to 20 carbon atoms within the above range, the flexibility of the intermediate layer can be improved and the heat seal strength can be improved. The content of units derived from ethylene and α-olefins having 4 to 20 carbon atoms is more preferably 12.0 to 40.0% by weight, even more preferably 13.0 to 40.0% by weight, and particularly preferably 15.0 to 36.0% by weight. The content of ethylene-derived units in the propylene-based thermoplastic elastomer (D) is preferably 6.0 to 20.0% by weight, and more preferably 8.0 to 18.0% by weight. The content of units derived from 1-butene in the propylene-based thermoplastic elastomer (D) is preferably 0 to 23.0% by weight, and more preferably 0 to 18.0% by weight. The total content of units derived from ethylene and 1-butene in the propylene-based thermoplastic elastomer (D) is preferably 8.0 to 40.0% by weight, more preferably 12.0 to 40.0% by weight, even more preferably 13.0 to 40.0% by weight, and particularly preferably 15.0 to 36.0% by weight.
[0039] (d4) can also be expressed as (d4') below. The content of units derived from (d4') ethylene and α-olefins having 4 to 20 carbon atoms is 12.0 to 40.0% by weight.
[0040] <<<Other ingredients>>> Other components may be incorporated into the intermediate layer, provided that they do not impair the effects of the present invention. Examples of such optional components include resins other than components (C) and (D), antioxidants, ultraviolet absorbers, nucleating agents, clearing agents, lubricants, antiblocking agents, antistatic agents, antifogging agents, neutralizing agents, light stabilizers, metal deactivators, colorants, dispersants, peroxides, fillers, fluorescent whitening agents, and the like, which are commonly used in polyolefin resin materials.
[0041] The proportion of other components to the total of 100% by weight of components (C) and (D) is preferably 10% by weight or less, more preferably 0.1 to 9% by weight, and even more preferably 0.5 to 8% by weight.
[0042] <Heat seal layer> The heat-seal layer is an unstretched polypropylene film, and the resin composition (B) constituting the heat-seal layer satisfies the following requirements (b1) and (b2). By satisfying the following requirements (b1) and (b2) of the resin composition (B), the heat-seal strength, low-temperature sealability, and bag drop resistance of the resulting laminated film can be improved. (b1) The durometer D hardness (HDD) measured in accordance with JIS K 7215:1986 is 10 to 78. (b2) Its melting point is 110-150°C.
[0043] <<Resin composition (B)>> The resin composition (B) satisfies the following requirements (b1) and (b2). (b1) The durometer D hardness (HDD) measured in accordance with JIS K 7215:1986 is 10 to 78. From the viewpoint of improving the heat seal strength of the laminated film, the durometer D hardness (HDD) of the resin composition (B) is preferably 10 to 78, more preferably 20 to 75, and more preferably 30 to 70.
[0044] (b2) Its melting point is 110-150°C. From the viewpoint of improving the heat seal strength, low-temperature sealability, and bag drop resistance of the laminated film, the melting point of the resin composition (B) is 110 to 150°C, preferably 110 to 140°C, more preferably 110 to 135°C, and even more preferably 110 to 130°C.
[0045] The resin composition (B) preferably further satisfies the following requirements (b3) to (b6).
[0046] (b3) In accordance with JIS K 7171:2022, the flexural modulus measured at a test speed of 2 mm / min is 10 to 1,300 MPa. From the viewpoint of improving the heat seal strength of the laminated film, the flexural modulus of the resin composition (B) is preferably 10 to 1,300 MPa, more preferably 100 to 1,000 MPa, even more preferably 200 to 900 MPa, and particularly preferably 300 to 800 MPa.
[0047] (b4) In accordance with JIS K 7127:1999, the Young's modulus in the machine direction (MD) measured at a tensile speed of 1 mm / min is 10 to 700 MPa. From the viewpoint of improving the heat seal strength of the laminated film, the Young's modulus of the resin composition (B) is preferably 10 to 700 MPa, more preferably 100 to 600 MPa, and even more preferably 200 to 500 MPa.
[0048] (b5) The heat of fusion ΔHm is 5 to 100 J / g. From the viewpoint of improving the heat seal strength of the laminated film, the heat of fusion ΔHm of the resin composition (B) is preferably 5 to 100 J / g, more preferably 10 to 90 J / g, and even more preferably 20 to 70 J / g.
[0049] (b6) The density measured at 23°C in accordance with JIS K 7112-2:2023 is 0.850 to 0.899 g / cm 3 . From the viewpoint of improving the heat seal strength of the laminated film, the density of the resin composition (B) is preferably 0.850 to 0.899 g / cm 3 , more preferably 0.860 to 0.895 g / cm 3 , and even more preferably 0.870 to 0.893 g / cm 3 .
[0050] From the viewpoint of improving heat seal strength and low-temperature sealing performance, the resin composition (B) contains a propylene polymer (E) and optionally a propylene thermoplastic elastomer (F). Preferably, the content of the propylene polymer (E) is 10 to 100% by weight and the content of the propylene thermoplastic elastomer (F) is 0 to 90% by weight, based on 100% by weight of the total of the propylene polymer (E) and the propylene thermoplastic elastomer (F). Furthermore, from the viewpoint of improving resistance to bag drop in addition to heat seal strength and low-temperature sealing performance, the content of component (E) based on 100% by weight of the total of component (E) and component (F) is more preferably 50 to 95% by weight, even more preferably 55 to 90% by weight, and particularly preferably 60 to 80% by weight. Similarly, the content of component (F) relative to 100% by weight of the total of component (E) and component (F) is more preferably 5 to 50% by weight, even more preferably 10 to 45% by weight, and particularly preferably 20 to 40% by weight.
[0051] <<<Propylene-based polymer (E)>>> The propylene polymer (E) is a copolymer of propylene and ethylene or an α-olefin having 4 to 20 carbon atoms, with a content of 0.1% by weight or more, and preferably satisfies the following requirements (e1) to (e5). The copolymer components with propylene, ethylene and α-olefins having 4 to 20 carbon atoms, may be one type or a combination of two or more types. The copolymer components are preferably ethylene or α-olefins having 4 to 10 carbon atoms. As ethylene and α-olefins having 4 to 20 carbon atoms, those exemplified in the propylene polymer (C) can be used. The propylene polymer (E) may also be a blend of two or more types of polymers: a propylene homopolymer and a random copolymer of propylene and ethylene or an α-olefin having 4 to 20 carbon atoms. The blend may be a melt blend obtained by melt-kneading these polymers that have been manufactured separately, or a polymer blend obtained as a multi-stage polymer produced by the multi-stage polymerization method described later. The propylene polymer (E) may be used alone or in combination of two or more types.
[0052] (e1) The MFR measured in accordance with JIS K 7210-1:2014 (230℃, 2.16kg load) is 1 to 50g / 10min. The propylene polymer (E) preferably has a melt flow rate (MFR) of 1 to 50 g / 10 min, measured in accordance with JIS K 7210-1:2014 (230°C, 2.16 kg load). More preferably, the MFR is 2 to 40 g / 10 min, and even more preferably 3 to 30 g / 10 min. Having an MFR of 1 to 50 g / 10 min for the propylene polymer (E) results in good compatibility with the propylene thermoplastic elastomer (F) and good film processability. Methods for controlling the MFR value are well known, and it can be easily adjusted by adjusting the temperature and pressure, which are polymerization conditions for propylene polymers (E), or by controlling the amount of chain transfer agents such as hydrogen added during polymerization.
[0053] (e2) In accordance with JIS K 7171:2022, the flexural modulus measured at a test speed of 2 mm / min is greater than 500 MPa and less than or equal to 1,300 MPa. The propylene polymer (E) preferably has a flexural modulus of elasticity exceeding 500 MPa and 1,300 MPa or less, as measured at a test speed of 2 mm / min in accordance with JIS K 7171:2022. The upper limit of the flexural modulus of elasticity is more preferably 1,200 MPa or less, and even more preferably 1,100 MPa or less. By setting the flexural modulus of elasticity to over 500 MPa, the moldability of the heat seal layer can be improved. By setting the flexural modulus of elasticity to 1,300 MPa or less, the flexibility of the heat seal layer can be maintained while improving the heat seal strength, low-temperature heat sealability, transparency, impact resistance, puncture resistance, tear strength, and resistance to bag drop at low temperatures. Methods for controlling the flexural modulus are well known, and it can be easily adjusted by controlling the content ratio of copolymerized ethylene and / or α-olefins having 4 to 20 carbon atoms.
[0054] (e3) The content of units derived from propylene is greater than 88.0% by weight and less than or equal to 99.9% by weight. The content of propylene-derived units in the propylene polymer (E) is preferably greater than 88.0% by weight and 99.9% by weight or less. By keeping the content of propylene-derived units within the above range, the flexibility of the heat seal layer can be maintained. The content of propylene-derived units is more preferably greater than 88.5% by weight and 98.0% by weight, and even more preferably greater than 89.0% by weight and 97.0% by weight.
[0055] (e4) The content of units derived from ethylene and α-olefins having 4 to 20 carbon atoms is 0.1% by weight or more and less than 12.0% by weight. The content of units derived from ethylene and α-olefins having 4 to 20 carbon atoms in the propylene polymer (E) is preferably 0.1% by weight or more and less than 12.0% by weight. By keeping the content of units derived from ethylene and α-olefins having 4 to 20 carbon atoms within the above range, the flexibility of the heat seal layer can be maintained. The content of units derived from ethylene and α-olefins having 4 to 20 carbon atoms is more preferably 2.0% by weight or less than 11.5% by weight, and even more preferably 3.0% by weight or less than 11.0% by weight. The content of ethylene-derived units in the propylene polymer (E) is preferably 0.1 to 7.0% by weight, and more preferably 1.0 to 5.0% by weight. The content of units derived from 1-butene in the propylene polymer (E) is preferably 0 to 11.0% by weight, and more preferably 0 to 10.0% by weight. The total content of units derived from ethylene and 1-butene in the propylene polymer (E) is preferably 0.1% by weight or more and less than 12.0% by weight, more preferably 2.0% to less than 11.5% by weight, and even more preferably 3.0% to less than 11.0% by weight.
[0056] (e5) Its melting point is 110-155°C. The melting point of the propylene polymer (E) is preferably 110 to 155°C, more preferably 115 to 145°C, and even more preferably 120 to 140°C. By setting the melting point in the range of 110 to 155°C, good low-temperature heat sealability can be achieved. Methods for controlling the melting point are well known, and it can be easily adjusted by controlling the content ratio of copolymerized ethylene and / or α-olefins having 4 to 20 carbon atoms.
[0057] From the viewpoint of imparting flexibility and low-temperature heat-sealability to the heat-seal layer, the propylene-based polymer (E) is preferably a propylene-ethylene copolymer or a propylene-ethylene-1-butene copolymer that satisfies the above requirements (e1) to (e5), and more preferably a propylene-ethylene-1-butene copolymer.
[0058] <<<Propylene-based thermoplastic elastomer (F)>>> The propylene-based thermoplastic elastomer (F) is preferably a copolymer of propylene and ethylene or an α-olefin having 4 to 20 carbon atoms, and satisfies the following requirements (f1) to (f4). The copolymer components with propylene, ethylene and α-olefins having 4 to 20 carbon atoms, may be one type or a combination of two or more types. The copolymer components are preferably ethylene or α-olefins having 4 to 10 carbon atoms. As ethylene and α-olefins having 4 to 20 carbon atoms, those exemplified in the propylene-based thermoplastic elastomer (D) can be used. Examples of propylene-based thermoplastic elastomers (F) include random copolymer rubbers of propylene and ethylene or α-olefins having 4 to 20 carbon atoms, specifically propylene-ethylene copolymers and propylene-ethylene-1-butene copolymers. The propylene-based thermoplastic elastomer (F) may be used alone or in combination of two or more types.
[0059] (f1) The MFR measured in accordance with JIS K 7210-1:2014 (230℃, 2.16kg load) is 1 to 30g / 10min. The propylene-based thermoplastic elastomer (F) preferably has an MFR of 1 to 30 g / 10 min, measured in accordance with JIS K 7210-1:2014 (230°C, 2.16 kg load). More preferably, the MFR is 2 to 20 g / 10 min, and even more preferably 2 to 10 g / 10 min. When the MFR of the propylene-based thermoplastic elastomer (F) is within the range of 1 to 30 g / 10 min, a film with good moldability and appearance can be obtained. Methods for controlling the MFR value are well known, and it can be easily adjusted by controlling the temperature and pressure, which are polymerization conditions for propylene-based thermoplastic elastomers (F), or by controlling the amount of chain transfer agents such as hydrogen added during polymerization.
[0060] (f2) The flexural modulus measured at a test speed of 2 mm / min in accordance with JIS K 7171:2022 is 5 to 200 MPa. The propylene-based thermoplastic elastomer (F) preferably has a flexural modulus of 5 to 200 MPa, measured at a test speed of 2 mm / min in accordance with JIS K 7171:2022. More preferably, the flexural modulus is 5 to 150 MPa, and even more preferably 5 to 100 MPa. If the flexural modulus is 5 MPa or higher, surface stickiness is suppressed during the molding of the heat seal layer, and if it is 200 MPa or lower, the flexibility of the heat seal layer is improved, resulting in improved heat seal strength, low-temperature heat sealability, transparency, impact resistance, puncture strength, tear strength, and resistance to bag drop at low temperatures. Methods for controlling the flexural modulus are well known, and it can be easily adjusted by controlling the content ratio of copolymerized ethylene and / or α-olefins having 4 to 20 carbon atoms.
[0061] (f3) The content of units derived from propylene is 60.0 to 92.0% by weight. The content of propylene-derived units in the propylene-based thermoplastic elastomer (F) is preferably 60.0 to 92.0% by weight. By setting the content of propylene-derived units within the above range, the flexibility of the heat seal layer is improved, and the heat seal strength, low-temperature heat sealability, transparency, impact resistance, puncture strength, tear strength, and low-temperature bag drop resistance can be improved. The content of propylene-derived units is more preferably 60.0 to 88.0% by weight, even more preferably 60.0 to 87.0% by weight, and particularly preferably 64.0 to 85.0% by weight.
[0062] (f3) can also be expressed as (f3') below. The content of units derived from (f3') propylene is 60.0 to 88.0% by weight.
[0063] (f4) The content of units derived from ethylene and α-olefins having 4 to 20 carbon atoms is 8.0 to 40.0% by weight. The content of units derived from ethylene and α-olefins having 4 to 20 carbon atoms in the propylene-based thermoplastic elastomer (F) is preferably 8.0 to 40.0% by weight. By setting the content of units derived from ethylene and α-olefins having 4 to 20 carbon atoms within the above range, the flexibility of the heat seal layer is improved, and the heat seal strength, low-temperature heat sealability, transparency, impact resistance, puncture strength, tear strength, and low-temperature bag drop resistance can be improved. The content of units derived from ethylene and α-olefins having 4 to 20 carbon atoms is more preferably 12.0 to 40.0% by weight, even more preferably 13.0 to 40.0% by weight, and particularly preferably 15.0 to 36.0% by weight. The content of ethylene-derived units in the propylene-based thermoplastic elastomer (F) is preferably 6.0 to 20.0% by weight, and more preferably 8.0 to 18.0% by weight. The content of units derived from 1-butene in the propylene-based thermoplastic elastomer (F) is preferably 0 to 23.0% by weight, and more preferably 0 to 18.0% by weight. The total content of units derived from ethylene and 1-butene in the propylene-based thermoplastic elastomer (F) is preferably 8.0 to 40.0% by weight, more preferably 12.0 to 40.0% by weight, even more preferably 13.0 to 40.0% by weight, and particularly preferably 15.0 to 36.0% by weight.
[0064] (f4) can also be expressed as (f4') below. (f4') The content of units derived from ethylene and α-olefins having 4 to 20 carbon atoms is 12.0 to 40.0% by weight.
[0065] <<<Other ingredients>>> Other components may be incorporated into the heat seal layer, provided that they do not impair the effects of the present invention. Examples of such optional components include resins other than components (E) and (F), antioxidants, ultraviolet absorbers, nucleating agents, clearing agents, lubricants, antiblocking agents, antistatic agents, antifogging agents, neutralizing agents, light stabilizers, metal deactivators, colorants, dispersants, peroxides, fillers, fluorescent whitening agents, and the like, which are commonly used in polyolefin resin materials.
[0066] The proportion of other components to the total of 100% by weight of components (E) and (F) is preferably 10% by weight or less, more preferably 0.1 to 9% by weight, and even more preferably 0.5 to 8% by weight.
[0067] (Origin of raw materials) In response to recent demands for reducing environmental impact, effectively utilizing resources, and building a sustainable society, the resins or raw materials constituting resin compositions (A) and (B) are not necessarily limited to unused materials (hereinafter referred to as "virgin materials"). In other words, recycled plastic (also called recycled resin or regenerated resin) can be used in at least part or all of the resins constituting resin compositions (A) and (B). Specifically, the resins constituting resin compositions (A) and (B) are not limited to consisting solely of virgin material; recycled plastic may be used alone, or virgin material and recycled plastic may be mixed in any proportion. The intended effects of the present invention can be achieved even when recycled plastic is used.
[0068] Here, "recycled plastic" broadly refers to resin materials that have been recycled from plastic waste generated during the manufacturing process or previously used, regardless of their manufacturing method or origin. While typically produced by the following methods, it is not limited to these. Furthermore, the presence or absence of third-party certification regarding its origin or recycling method is irrelevant. (1) Material recycling (mechanical recycling): This method involves recycling used plastic products while substantially maintaining their polymer structure through physical processing such as crushing, washing, drying, deodorizing, sorting, foreign matter removal, melting and kneading, and re-pelletization. Used plastic products may be either post-consumer recycled (PCR) materials recovered from products used by consumers, or post-industrial recycled (PIR) materials recovered from manufacturing processes such as scraps and off-spec products. (2) Chemical recycling (feedstock recycling): This method involves decomposing used plastic products into monomers, oligomers, synthesis gas, or derived oils by chemical means such as thermal decomposition, gasification, and depolymerization, and then polymerizing these to obtain recycled plastics. This method also includes cases where raw materials derived from used plastics and raw materials derived from fossil fuels are mixed and used in specific manufacturing facilities or processes, and the proportion derived from recycled plastics is allocated using a mass balance method (material balance method). Furthermore, the recycled plastics described above can be in any form, such as pellets, powder, or flakes. Any of these recycled plastics can be used in the production of resin compositions (A) and (B) using the same manufacturing process and conditions as virgin materials, and additional steps such as drying and deodorization may be added as needed.
[0069] Furthermore, at least part or all of the raw materials for the resins constituting resin compositions (A) and (B) can be biomass-derived raw materials (hereinafter referred to as "biomass raw materials"). Specifically, the raw materials for the resins constituting resin compositions (A) and (B) are not limited to consisting solely of components derived from fossil fuels (hereinafter also referred to as "fossil raw materials"), but may consist solely of biomass raw materials, or fossil raw materials and biomass raw materials may be mixed in any proportion. The intended effects of the present invention can be achieved even when biomass raw materials are used.
[0070] Here, "biomass raw materials" broadly refers to renewable natural resources such as plants, animals, fungi, yeasts, algae, and bacteria, as well as their residues, that are used as raw materials. Any of these raw materials can be obtained by any conventionally known method. This also includes cases where biomass raw materials and fossil raw materials are mixed and used in specific manufacturing facilities or processes, and the proportion of biomass raw materials is allocated using a mass balance method. Furthermore, it does not require any third-party certification regarding the origin or recycling method.
[0071] If the manufacturing conditions, such as polymerization catalysts and polymerization temperatures, are equivalent, the molecular structure of the resin obtained using biomass raw materials will be: 14 Except for the proportion of C isotopes, it is equivalent to resin obtained from fossil raw materials. Therefore, the performance of resin obtained from biomass raw materials is also substantially the same as that of resin obtained from fossil raw materials. In other words, the resins constituting resin compositions (A) and (B) can be produced from the above biomass raw materials using the same manufacturing equipment and manufacturing conditions that were used for conventional fossil raw materials.
[0072] (Method for producing propylene polymers (C) and (E)) Polymerization catalysts for producing propylene polymers (C) and (E) include Ziegler-Natta catalysts and / or metallocene catalysts, but other catalysts may also be used. The Ziegler-Natta catalyst is described in Section 2.3.1 (pages 20-57) of the "Polypropylene Handbook," edited by Edward P. Moore Jr., translated and supervised by Tetsuo Yasuda and Nobu Sakuma, published by Kogyo Chosakai (1998). The Ziegler-Natta catalyst includes (1) a combination of titanium trichloride catalysts consisting of titanium trichloride and organoaluminum halides, magnesium chloride, and titanium halides; (2) a magnesium-supported catalyst consisting of a solid catalyst component containing an electron-donating compound and organoaluminum and organosilicon compounds; and (3) a catalyst combining an organoaluminum compound component with an organosilicon-treated solid catalyst component formed by contacting a solid catalyst component with organoaluminum and organosilicon compounds.
[0073] The metallocene catalyst is a catalyst comprising (i) a transition metal compound of Group 4 of the periodic table containing a ligand having a cyclopentadienyl skeleton (a so-called metallocene compound), (ii) a co-catalyst that can be activated to a stable ionic state by reacting with the metallocene compound, and optionally (iii) an organoaluminum compound. Any known catalyst can be used. The metallocene compound is preferably a crosslinked metallocene compound capable of stereoregular polymerization of propylene, and more preferably a crosslinked metallocene compound capable of isoregular polymerization of propylene.
[0074] (i) As metallocene compounds, those disclosed in Japanese Patent Publication Nos. S60-35007, S61-130314, S63-295607, H1-275609, H2-41303, H2-131488, H2-76887, H3-163088, H4-300887, H4-211694, H5-43616, H5-209013, H6-239914, H7-504934, and H8-85708 can be preferably used.
[0075] Specifically, methylenebis(2-methylindenyl)zirconium dichloride, ethylenebis(2-methylindenyl)zirconium dichloride, ethylene 1,2-(4-phenylindenyl)(2-methyl-4-phenyl-4H-azlenyl)zirconium dichloride, isopropylidene(cyclopentadienyl)(fluorenyl)zirconium dichloride, isopropylidene(4-methylcyclopentadienyl)(3-t-butylindenyl)zirconium dichloride, dimethylsilylene(2-methyl-4-t-butyl-cyclopentadienyl)(3'-t-butyl-5'-methyl-cyclopentadienyl)zirconium dichloride, dimethylsilylenebis(indenyl Zirconium dichloride, dimethylsilylenebis(4,5,6,7-tetrahydroindenyl) zirconium dichloride, dimethylsilylenebis[1-(2-methyl-4-phenylindenyl)] zirconium dichloride, dimethylsilylenebis[1-(2-ethyl-4-phenylindenyl)] zirconium dichloride, dimethylsilylenebis[4-(1-phenyl-3-methylindenyl)] zirconium dichloride, dimethylsilylene(fluorenyl)t-butylamide zirconium dichloride, methylphenylsilylenebis[1-(2-methyl-4,(1-naphthyl)-indenyl)] zirconium dichloride, dimethylsilylenebis[1-(2-methyl-4,5-Benzoindenyl) Zirconium dichloride, dimethylsilylenebis[1-(2-methyl-4-phenyl-4H-azlenyl)] Zirconium dichloride, dimethylsilylenebis[1-(2-ethyl-4-(4-chlorophenyl)-4H-azlenyl)] Zirconium dichloride, dimethylsilylenebis[1-(2-ethyl-4-naphthyl-4H-azlenyl)] Zirconium dichloride, diphenylsilylenebis[1-(2-methyl-4-(4-chlorophenyl)-4H-azlenyl)] Zirconium dichloride, diphenylsilylenebis[1-(2-methyl-4-(4-chlorophenyl)-4H-azlenyl] Examples of zirconium compounds include phenyl)-4H-azlenyl) zirconium dichloride, dimethylsilylenebis[1-(2-ethyl-4-(3-fluorobiphenylyl)-4H-azlenyl) zirconium dichloride, dimethylgermylenebis[1-(2-ethyl-4-(4-chlorophenyl)-4H-azlenyl) zirconium dichloride, and dimethylgermylenebis[1-(2-ethyl-4-phenylindenyl) zirconium dichloride.
[0076] Compounds in which zirconium is replaced with titanium, hafnium, etc., can also be used in the same manner. It is also preferable to use a mixture of zirconium compounds and hafnium compounds, etc. Furthermore, the chloride can be replaced with other halogen compounds, hydrocarbon groups such as methyl, isobutyl, and benzyl, amide groups such as dimethylamide and diethylamide, alkoxide groups such as methoxy and phenoxy groups, hydride groups, etc. Of these, metallocene compounds in which an indenyl group or an azlenyl group is crosslinked with silicon or a gelmyl group are particularly preferred.
[0077] Furthermore, metallocene compounds may be used supported on an inorganic or organic compound carrier. Preferred carriers are porous inorganic or organic compounds, specifically inorganic compounds such as ion-exchangeable layered silicates, zeolites, SiO2, Al2O3, silica alumina, MgO, ZrO2, TiO2, B2O3, CaO, ZnO, BaO, and ThO2; and organic compounds consisting of porous polyolefins, styrene-divinylbenzene copolymers, olefin-acrylic acid copolymers, etc., or mixtures thereof.
[0078] (ii) Preferred co-catalysts that can react with metallocene compounds to activate them into a stable ionic state include organoaluminum oxy compounds (e.g., aluminoxane compounds), ion-exchangeable layered silicates, Lewis acids, boron-containing compounds, ionic compounds, fluorine-containing organic compounds, and the like.
[0079] (iii) Preferred organoaluminum compounds include trialkylaluminum such as triethylaluminum, triisopropylaluminum, and triisobutylaluminum, dialkylaluminum halides, alkylaluminum sesquihalides, alkylaluminum dihalides, alkylaluminum hydrides, and organoaluminum alkoxides.
[0080] There are no particular restrictions on the method for producing the propylene polymers (C) and (E). They can be produced using any of the conventionally known slurry polymerization methods, bulk polymerization methods, gas-phase polymerization methods, etc. Furthermore, within the limits, it is also possible to produce the propylene polymers (C) and (E) using multi-stage polymerization methods.
[0081] (Methods for producing propylene-based thermoplastic elastomers (D) and (F), etc.) Examples of propylene-based thermoplastic elastomers (D) and (F) include propylene-1-butene copolymer described in Japanese Patent Publication No. 2004-099909; propylene-ethylene-1-butene copolymer described in Japanese Patent Publication No. 2004-315830, Japanese Patent Publication No. 2007-169666, and Japanese Patent Publication No. 2010-163626; propylene-α-olefin copolymer described in Japanese Patent Publication No. 2022-152305 and Japanese Patent Publication No. 2022-152304, etc.
[0082] (Method for calculating the content ratio of units derived from ethylene and α-olefins with 4 to 20 carbon atoms) The content ratio of units derived from ethylene and α-olefins having 4 to 20 carbon atoms in propylene polymers (C) and (E) and propylene thermoplastic elastomers (D) and (F) is as follows: 13This can be determined from the integrated intensity of the spectrum obtained by 13C-NMR measurement. For example, in the case of propylene-ethylene-1-butene copolymer, the content (weight %) of ethylene and 1-butene can be determined from (Equation-1) and (Equation-2) below, respectively. Ethylene content (mol%) = IE × 100 / (IE + IP + IB) Ethylene content (weight %) = [Ethylene content (mol%) × Molecular weight of ethylene] / [Ethylene content (mol%) × Molecular weight of ethylene + Propylene content (mol%) × Molecular weight of propylene + 1-butene content (mol%) × Molecular weight of 1-butene] ... (Equation 1) 1-Butene content (mol%) = IB × 100 / (IE + IP + IB) 1-Butene content (weight %) = [1-Butene content (mol%) × Molecular weight of 1-Butene] / [Ethylene content (mol%) × Molecular weight of ethylene + Propylene content (mol%) × Molecular weight of propylene + 1-Butene content (mol%) × Molecular weight of 1-Butene] ... (Equation 2) Here, IE, IP, and IB are the integrated intensities of carbon derived from ethylene, propylene, and 1-butene, respectively.
[0083] <Base material layer> The base layer is a stretched polypropylene film. The base layer functions as a layer that provides the laminated film with a predetermined strength. By using a stretched polypropylene film as the base layer, the strength of the laminated film is improved, and in combination with the intermediate layer and the heat seal layer, it can be suitably used as a monomaterial packaging material, and the laminated film can be made recyclable. The base layer may be a uniaxially oriented polypropylene film or a biaxially oriented polypropylene film, but from the viewpoint of versatility, a biaxially oriented polypropylene film is preferred.
[0084] Examples of polypropylene constituting the base layer include propylene homopolymers, random copolymers of propylene and ethylene or α-olefins having 4 to 20 carbon atoms, and block copolymers of propylene and ethylene or α-olefins having 4 to 20 carbon atoms. The base layer may be composed of one type of polypropylene or two or more types of polypropylene. From the viewpoint of the strength and secondary processability of the laminated film, the base layer preferably contains 80% by weight or more of units derived from propylene, more preferably 90% by weight or more, and even more preferably 95% by weight or more. The base layer is particularly preferably a propylene homopolymer.
[0085] Other components may be incorporated into the base layer as long as they do not impair the effects of the present invention. Examples of such optional components include those exemplified as other components in the intermediate layer and heat seal layer. Furthermore, similar to the resins constituting the intermediate layer and heat seal layer, the resin constituting the base layer is not limited to consisting solely of virgin material, but may consist solely of recycled plastic and / or biomass raw materials, or it may be a mixture of virgin material and recycled plastic and / or biomass raw materials in any proportion.
[0086] (Method for producing the base layer and intermediate layer) Unstretched polypropylene films, including the base layer and intermediate layer, can be manufactured by conventionally known methods. For example, an unstretched polypropylene film can be obtained by heating, melting, and kneading the raw resin in an extruder, then extruding it into a film or sheet from a T-die. When using multiple raw resins, the raw resins may be dry-blended or melt-kneaded beforehand to form pellets, etc., and then extruded into a film or sheet from a T-die to obtain the base layer and intermediate layer. The obtained unstretched polypropylene film can then be stretched to obtain a stretched polypropylene film. The method for manufacturing a laminate of stretched polypropylene films for a base layer and an intermediate layer is not particularly limited. For example, methods include manufacturing the stretched polypropylene films for the base layer and the intermediate layer separately and then bonding them together by a dry lamination method, or manufacturing a laminate of unstretched polypropylene films by laminating the base layer and the intermediate layer using a co-extrusion method, and then stretching the laminate.
[0087] Publicly known methods can be used for stretching, such as the tubular stretching method, the tenter stretching method, and the pantograph batch stretching method.
[0088] The stretching direction is not particularly limited, but is usually longitudinal and / or transverse. In the case of uniaxial stretching, it may be longitudinal or transverse uniaxial stretching, for example, by utilizing the difference in roll peripheral speed. The stretching temperature is preferably 90 to 140°C, and more preferably 100 to 130°C. The stretching ratio is preferably 3 to 12 times, and more preferably 4 to 12 times.
[0089] In the case of biaxial stretching, either sequential or simultaneous biaxial stretching is acceptable. One example of a stretching method is to roll-stretch a sheet obtained by the T-die method to a length of 3.0 to 6.0 times in the longitudinal (MD) direction, and then stretch it to a length of 8.0 to 12.0 times in the transverse (TD) direction using the tenter method. Another example of a stretching method is the so-called tubular stretching method, in which a tubular unstretched sheet obtained from an annular die by air cooling or water cooling is heated below its melting point, and then stretched by air in a bubble-like manner by 3.0 to 7.0 times in the longitudinal (MD) direction and 3.0 to 7.0 times in the transverse (TD) direction. In the case of biaxial stretching, the stretching temperature is preferably 100°C to 170°C, and more preferably 110°C to 160°C.
[0090] Stretched polypropylene film can be surface-treated to improve its printability, lamination properties, etc. Examples of surface treatment methods include corona discharge treatment, plasma treatment, flame treatment, and acid treatment, and there are no particular limitations. Corona discharge treatment, plasma treatment, or flame treatment are preferred because they allow for continuous processing and can be easily performed before the winding process in the film's manufacturing process.
[0091] (Method for creating a heat-sealed layer) The heat seal layer can be manufactured by conventionally known methods. For example, the raw material resin can be heated, melted, and kneaded in an extruder, and then extruded from a T-die into a film or sheet to obtain the heat seal layer. Alternatively, the melted and kneaded raw material resin can be processed into pellets, etc., and then extruded from a T-die into a film or sheet to obtain the heat seal layer. The heat seal layer may be subjected to corona treatment or the like.
[0092] <Laminated film> The laminated film is formed by laminating a base layer, an intermediate layer, and a heat-seal layer in this order. From the viewpoint of moldability and film properties, the thickness of the intermediate layer is preferably 1 to 10 μm, more preferably 1 to 5 μm, and even more preferably 1 to 3 μm. From the viewpoint of heat-seal strength, the thickness of the heat-seal layer is preferably 10 to 400 μm, more preferably 20 to 150 μm, and even more preferably 30 to 100 μm. From the viewpoint of moldability and film properties, the thickness of the base layer is preferably 9 to 475 μm, more preferably 15 to 80 μm, and even more preferably 20 to 70 μm. The total thickness of the laminated film is preferably 17 to 500 μm, more preferably 35 to 200 μm, and even more preferably 50 to 150 μm.
[0093] The laminated film may include layers other than the base layer, intermediate layer, and heat-seal layer, as long as the effects of the present invention are not impaired. Examples of other layers include a scratch-resistant layer, a printed layer, an adhesive layer, a barrier layer, a gas permeable layer, a gas adsorption layer, and a vapor-deposited layer using aluminum, silica, etc.
[0094] [Physical properties of laminated films] The laminated film preferably has a sealing temperature of 140°C or lower, more preferably 80°C to 135°C, and even more preferably 90°C to 130°C, at which a heat seal strength of 20 N / 15 mm is achieved, as measured under the following conditions. By setting the sealing temperature to 140°C or lower, low-temperature sealing performance can be improved. As a result, it becomes possible to improve production speed by shortening the sealing time, lower the temperature setting of the sealing bar, and improve secondary processability by reducing shrinkage of the laminated film during bonding. The sealing temperature can be achieved by changing the type and blending ratio of the resin constituting the heat seal layer, changing the type of resin in the base layer and intermediate layer, or adjusting the thickness ratio of the base layer, intermediate layer and heat seal layer. <Measurement of sealing temperature at which a heat seal strength of 20 N / 15 mm is reached> After storing the laminated film at an ambient temperature of 23°C for 7 days, it is cut into strips measuring 180 mm (MD) x 80 mm (TD). The MD section is folded in half so that the heat-seal layers are in contact with each other, and heat-sealed at a position 20-30 mm from the fold, with a width of 10 mm, under the following sealing conditions. The obtained partially heat-sealed sample is cut into strips so that the TD section is 15 mm wide to obtain a test specimen. The obtained test specimen is pulled at both ends of the specimen in a 180° peeling direction using a Shopper-type tensile testing machine at a speed of 500 mm / min, and the maximum force required to peel off the heat-sealed portion is measured and defined as the heat seal strength. The sealing conditions are: sealing pressure: 2.0 kg / cm² 2 (0.196 MPa), sealing time: 1.0 second, sealing temperature: 90°C to 170°C in 10°C increments. In the seal curve obtained from the seal temperature and heat seal strength, the data points at any two points where the seal temperature was measured at 10°C intervals are approximated by a linear function to determine the seal temperature at which the heat seal strength reaches 20 N / 15 mm.
[0095] The laminated film preferably has a haze of less than 10%, as measured in accordance with JIS K 7136:2000. A haze of less than 10% improves the transparency of the laminated film. A haze of 0.5-9% is more preferable, and 1-8% is even preferable. If the haze is less than 0.5%, the surface irregularities of the laminated film become smaller, causing excessive adhesion (blocking) between the films, which can worsen the ability to perform secondary processing.
[0096] The laminated film preferably has a puncture strength of 10N or higher, more preferably 11N or higher, and even more preferably 12N or higher, as measured in accordance with JIS Z 1707:2019. The upper limit of the puncture strength is not particularly limited, but is usually 20N or lower. If the puncture strength is less than 10N, the laminated film may crack and the bag may rupture during secondary processing or market distribution.
[0097] In a bag drop impact test measured under the following conditions, the laminated film preferably has an average number of bag breakages of 6 or more, more preferably 10 or more, and even more preferably 20 or more. The average number of bag breakages is rounded down to the nearest integer. <Bag impact test> Two 120mm x 150mm sheets are cut from the laminated film, the heat-sealed layers of each sheet are overlapped, and three sides are sealed using an impulse sealer under the following sealing conditions to create a 120mm x 150mm sample bag. 100ml of water is added to the sample bag, and the open side is sealed using an impulse sealer under the following sealing conditions to create a water-sealed test specimen. The water-sealed test specimen is stored in a 0°C atmosphere for one day, then dropped 50 times consecutively from a height of 1.5m onto a metal plate. The maximum number of times the bag did not rupture is recorded as the number of rupture drops. The test is repeated 5 times, and the average number of rupture drops is calculated. The sealing conditions are as follows: using a Fuji Impulse Poly Sealer (product name: PC-300), with a sealing width of 2 mm and a scale of 10 (sealing time of 1.6 seconds).
[0098] <Method for manufacturing laminated film> The method for bonding the base layer, intermediate layer, and heat seal layer is not particularly limited, and conventionally known methods can be used. For example, the adhesive layer can be formed by extrusion, dry lamination, etc., to bond the base layer to the intermediate layer and the intermediate layer to the heat seal layer. The order of bonding the base layer to the intermediate layer and the intermediate layer to the heat seal layer is not particularly limited, but from the viewpoint of productivity, it is preferable to bond the intermediate layer to the heat seal layer after obtaining a laminate in which the base layer and intermediate layer have been bonded. In particular, a manufacturing method comprising the steps of obtaining a laminate by co-extruding a base layer and an intermediate layer, obtaining a stretched film by stretching the laminate obtained in step 1, and adhering a heat-seal layer onto the intermediate layer of the stretched film obtained in step 2 is preferred from the viewpoint of obtaining high adhesive strength, fast processing speed, and high productivity. Furthermore, dry lamination, extrusion lamination, and the like can be used as the bonding method in step 3. From the viewpoint of being able to laminate a wide variety of materials and impart diverse functionalities, it is preferable that step 3 is a step in which the intermediate layer and the heat seal layer are bonded by dry lamination.
[0099] In the dry lamination method, the adhesive may be applied to the intermediate layer before bonding the heat-seal layer, or the adhesive may be applied to the heat-seal layer before bonding the intermediate layer. The adhesive may also be produced from an adhesive composition prepared by mixing a first composition containing a main component and a solvent with a second composition containing a curing agent and a solvent. Specifically, the adhesive includes a cured product produced by the reaction of the main component and the curing agent in the adhesive composition.
[0100] Examples of adhesives include polyurethane. Polyurethane is a cured product of a polyol, which is the main component, reacting with an isocyanate compound, which is the curing agent. Examples of polyurethane include polyether polyurethane and polyester polyurethane. Polyether polyurethane is a cured product produced by the reaction of a polyether polyol, which is the main component, with an isocyanate compound, which is the curing agent. Polyester polyurethane is a cured product produced by the reaction of a polyester polyol, which is the main component, with an isocyanate compound, which is the curing agent. As isocyanate compounds, aromatic isocyanate compounds such as tolylene diisocyanate (TDI), 4,4'-diphenylmethane diisocyanate (MDI), and xylylene diisocyanate (XDI); aliphatic isocyanate compounds such as hexamethylene diisocyanate (HDI) and isophorone diisocyanate (IPDI); or adducts or polymers of the above isocyanate compounds can be used.
[0101] The thickness of the adhesive layer is not particularly limited, but is preferably in the range of 0.01 to 5 μm, more preferably in the range of 0.03 to 3 μm, and particularly preferably in the range of 0.05 to 2 μm. If the thickness of the adhesive layer is greater than or equal to the lower limit above, more sufficient interlayer adhesion strength can be obtained.
[0102] <Applications of laminated films> Because the laminated film has excellent heat seal strength and low-temperature sealability, it can be suitably used for food packaging films, heavy product packaging films, and liquid packaging films, particularly for rice bags and individual packaging of frozen foods. [Examples]
[0103] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these examples. The raw materials used in the examples and the evaluation method for the obtained films are as follows.
[0104] 1. Evaluation Method (1) MFR The MFR of the raw resin was measured in accordance with JIS K 7210-1:2014 (230°C, 2.16 kg load).
[0105] (2) Melting point (Tm) and heat of fusion (ΔHm) For the raw material resin, resin composition (A), and resin composition (B), a differential scanning calorimeter (DSC) was used to heat a 5.0 mg sample to 200°C, hold it at 200°C for 5 minutes, and then lower the temperature to 40°C at a rate of 10°C / min. Subsequently, the top temperature of the endothermic peak when the sample was heated at a rate of 10°C / min was defined as the melting point (Tm), and the peak area of that peak was defined as the heat of fusion (ΔHm). The unit of ΔHm is J / g.
[0106] (3) Flexural modulus Injection-molded test specimens with a thickness of 4.0 mm, a width of 10.0 mm, and a length of 80 mm were prepared for the raw material resin, resin composition (A), and resin composition (B). The test specimens were prepared using a Toshiba Machine Co., Ltd. IS80G injection molding machine, molded at a molding temperature of 200°C and a mold temperature of 40°C, to form dumbbell-shaped tensile test specimens (Type A). Using these specimens, the flexural modulus was measured at a test speed of 2 mm / min in accordance with JIS K 7171:2022 (ISO 178). The unit of flexural modulus is MPa.
[0107] (4) Durometer D hardness (HDD) Test specimens (4 mm thick) were prepared by molding the raw material resin, resin composition (A), and resin composition (B) using a Toshiba Machine Co., Ltd. IS80G injection molding machine at a molding temperature of 200°C and a mold temperature of 40°C. The hardness of these test specimens was measured using a Type D durometer in accordance with JIS K 7215:1986.
[0108] (5) Young's modulus (MD) Test specimens were prepared for the raw material resin, resin composition (A), and resin composition (B) as follows. For resin composition (A) and resin composition (B), the propylene polymer and propylene thermoplastic elastomer constituting each composition were mixed in a blender in predetermined proportions, and then melt-extruded at 230°C to form pellets. For the raw material resin, the pellets were used as is. The obtained pellets were melt-extruded from a T-die mounted on an extruder with a diameter of 35 mm at a resin temperature of 240°C and a width of 320 mm to form an unstretched film with a thickness of 50 μm. From the obtained unstretched film, strip-shaped test specimens with a flow direction (MD): 150 mm and transverse direction (TD): 15 mm were cut. Using these test specimens, the Young's modulus (tensile modulus) of the MD was measured in accordance with JIS K 7127:1999, with a chuck distance of 100 mm and a crosshead speed of 1 mm / min. The unit of Young's modulus is MPa.
[0109] (6) Density Test specimens were prepared by molding the raw material resin, resin composition (A), and resin composition (B) using a Toshiba Machine Co., Ltd. IS80G injection molding machine at a molding temperature of 200°C and a mold temperature of 40°C. The density of these test specimens was measured at 23°C in accordance with JIS K7112-2:2023.
[0110] (7) Ethylene and 1-butene content The ethylene and 1-butene content in the propylene polymer and propylene thermoplastic elastomer used as raw materials is 13 The intensity was determined from the integrated intensity of the spectrum obtained by 13C-NMR measurement. The sample preparation and NMR measurement conditions are as follows. 200 mg of a propylene polymer or propylene thermoplastic elastomer was dissolved in 2.4 ml of o-dichlorobenzene / deuterated bromidebenzene (C6D5Br) = 4 / 1 (volume ratio) and hexamethyldisiloxane, a reference substance for chemical shift, in an NMR sample tube with an inner diameter of 10 mmφ. NMR measurements were performed using a Bruker BioSpin AV400 NMR spectrometer equipped with a 10 mmφ cryoprobe. 13 ¹³C-NMR measurements were performed with a sample temperature of 120°C, a pulse angle of 90°, a pulse interval of 15 seconds, and a total of 512 integrations. The ethylene content (weight%) and 1-butene content (weight%) of propylene polymers and propylene thermoplastic elastomers are as follows: 13 The integral intensities of the spectra obtained by 13C-NMR measurements were used to determine the following (Equation-1) and (Equation-2), respectively. Ethylene content (mol%) = IE × 100 / (IE + IP + IB) Ethylene content (weight %) = [Ethylene content (mol%) × Molecular weight of ethylene] / [Ethylene content (mol%) × Molecular weight of ethylene + Propylene content (mol%) × Molecular weight of propylene + 1-butene content (mol%) × Molecular weight of 1-butene] ... (Equation 1) 1-Butene content (mol%) = IB × 100 / (IE + IP + IB) 1-Butene content (weight %) = [1-Butene content (mol%) × Molecular weight of 1-Butene] / [Ethylene content (mol%) × Molecular weight of ethylene + Propylene content (mol%) × Molecular weight of propylene + 1-Butene content (mol%) × Molecular weight of 1-Butene] ... (Equation 2) Here, IE, IP, and IB are the integrated intensities of carbon derived from ethylene, propylene, and 1-butene, respectively.
[0111] (8) Maximum heat seal strength (unit: N / 15mm) The laminated films obtained in the examples and comparative examples were stored at an ambient temperature of 23°C for 7 days, then cut into strips measuring 180 mm (MD) x 80 mm (TD). The MD portion was folded in half so that the heat-seal layers were in contact with each other, and heat-sealed at a position 20-30 mm from the fold, with a width of 10 mm, under the following sealing conditions. The obtained partially heat-sealed samples were cut into strips with a TD width of 15 mm to obtain test specimens. The obtained test specimens were pulled at both ends of the specimen in a 180° peeling direction at a speed of 500 mm / min using a Shopper-type tensile testing machine (manufactured by Tester Industries Co., Ltd.), and the maximum force required to peel off the heat-sealed portion was measured and defined as the heat seal strength. The sealing conditions are: sealing pressure: 2.0 kg / cm². 2 (0.196 MPa), sealing time: 1.0 second, sealing temperature: set in 10°C increments within the range of 90°C to 170°C. After obtaining a seal curve from the seal temperature and heat seal strength, the average of the heat seal strengths between 140°C and 170°C was defined as the maximum heat seal strength. A maximum heat seal strength of 40 N / 15 mm or higher was considered to indicate superior heat seal strength.
[0112] (9) Heat seal start temperature (unit: °C) In the sealing curve obtained using the method for achieving maximum heat seal strength in the range of 90°C to 170°C, the data points at any two points measured at 10°C intervals were approximated by a linear function, and the sealing temperature at which the heat seal strength reached 20 N / 15 mm was defined as the heat seal start temperature. The lower this temperature, the faster the heat seal strength rises, indicating a film with good low-temperature heat sealability. A heat seal start temperature of 140°C or lower was judged to indicate excellent low-temperature heat sealability.
[0113] (10) Dropping bag impact test (resistance to dropping bags at low temperatures) Two 120mm x 150mm sheets were cut from the laminated films obtained in the examples and comparative examples. The heat-sealed layers of each sheet were overlapped, and three sides were sealed using an impulse sealer under the following sealing conditions to create a 120mm x 150mm sample bag with a 116mm opening. 100mL of water was poured into the opening of the sample bag, and the open side was sealed using an impulse sealer under the following sealing conditions to create a water-sealed test specimen. The water-sealed test specimen was stored in a 0°C atmosphere for one day, and then dropped 50 times consecutively from a height of 1.5m onto a metal plate. The maximum number of times the bag did not rupture was defined as the number of rupture drops. The test was repeated 5 times, and the average number of rupture drops was calculated. The average number of rupture drops was rounded down to an integer and used as an index of drop resistance at low temperatures. The sealing conditions were as follows: Fuji Impulse's Poly Sealer "Product Name: PC-300", with a sealing width of 2 mm and a scale of 10 (sealing time of 1.6 seconds). A bag was judged to have excellent resistance to bag breakage if the average number of bag breakages was 20 or more.
[0114] (11) Film thickness The thickness of the laminated films obtained in the examples and comparative examples was measured using a thickness gauge (manufactured by Mitutoyo Corporation).
[0115] (12) Haze (Transparency) (Unit: %) The haze of the laminated films obtained in the examples and comparative examples was measured in accordance with JIS K 7136:2000. A haze of less than 10% was considered to indicate excellent transparency.
[0116] (13) Puncture strength (unit: N) For the laminated films obtained in the examples and comparative examples, in accordance with JIS Z 1707:2019, test specimens were fixed with the substrate layer facing upwards, and a semicircular needle with a diameter of 1.0 mm and a tip radius of 0.5 mm was pierced at a speed of 50 ± 5 mm per minute. The maximum stress until the needle penetrated was measured and defined as the puncture strength (N). A puncture strength of 10 N or higher was considered to indicate excellent puncture strength.
[0117] (14) Recyclability In the examples and comparative examples, if each layer constituting the laminated film was a polypropylene film, it was marked as recyclable ("○"), and if not, it was marked as "×".
[0118] 2.Raw materials Manufacturing Example 1: Production of Propylene Polymer-1 A propylene-ethylene-1-butene copolymer was produced using a Ziegler-Natta catalyst as described below.
[0119] [Preparation of catalyst component (A)] As component (A1), THC-C-125 purchased from Toho Titanium Co., Ltd. was used. Analysis of component (A1) revealed that it contained 1.9 mass% Ti, 20.2 mass% Mg, and 63.7 mass% Cl. Next, a 20L autoclave equipped with a stirring device was thoroughly purged with nitrogen, and 100g of the slurry of component (A1) was introduced as component (A1). Purified n-heptane was introduced, and the concentration of component (A1) was adjusted to 25 g / L. 50 ml of silicon tetrachloride was added, and the reaction was carried out at 90°C for 1 hour. The reaction product was thoroughly washed with purified n-heptane. Subsequently, purified n-heptane was introduced to adjust the liquid level to 4 L. To the slurry of the reaction product of component (A1) obtained in this way, 30 ml of dimethyldivinylsilane as a vinylsilane compound (component (A2)), 30 ml of diisopropyldimethoxysilane as an organosilicon compound (component (A3)), and a diluted solution of triethylaluminum in n-heptane containing 80 g of triethylaluminum as an organoaluminum compound (component (A4)) were added, and the reaction was carried out at 40°C for 2 hours. The reaction product was thoroughly washed with purified n-heptane, and a portion of the resulting slurry was sampled and dried. Analysis revealed that the obtained catalyst component (A) contained 0.88% by mass of Ti, 8.0% by mass of diisopropyldimethoxysilane, and 63.7% by mass of chlorine.
[0120] [Prepolymerization] Using the component (A) obtained above, prepolymerization was carried out according to the following procedure. Purified n-heptane was introduced into the slurry of component (A) to adjust the concentration of component (A) to 20 g / L. After cooling the slurry to 10°C, a dilution of triethylaluminum in n-heptane containing 10 g of triethylaluminum was added, and 280 g of propylene was supplied over 4 hours. After the supply of propylene ran out, the reaction was continued for another 30 minutes. Next, the gas phase was thoroughly replaced with nitrogen, and the reaction product was thoroughly washed with purified n-heptane. The obtained slurry was removed from the autoclave and vacuum-dried to obtain component (A) after prepolymerization. This prepolymerized component (A) contained 2.0 g of polypropylene per gram of solid component. After prepolymerization, component (A) was slurryed with n-hexane, and the amount needed for approximately one week of continuous operation was added to the catalyst feed tank. No additional additions were made during operation.
[0121] [Polymerization process] Propylene polymer-1 was manufactured using the process flow shown in Figure 1. The process flow shown in Figure 1 will be explained below. In a horizontal polymerizer 5 (L / D=4.3, internal volume 100 liters) equipped with stirring blades, 0.14 g / h of the above pre-polymerized component (A) and a propylene polymerization catalyst prepared by adding triethylaluminum as an organoaluminum compound (component (B)) so that the Al / Mg molar ratio was 10 relative to the Mg in pre-polymerized component (A) were continuously supplied from piping 1. The reaction temperatures were set at 58°C, 61°C, and 64°C for each of the three equally divided volumes of the horizontal polymerization chamber 5, starting from the upstream side. While maintaining reaction pressure of 1.90 MPa and stirring speed of 28 rpm, hydrogen gas and ethylene were continuously supplied from circulation pipe 2, and 1-butene from pipe 3, to adjust the polymer's MFR, ethylene content, and 1-butene content, maintaining the hydrogen concentration in the gas phase of the polymer at the hydrogen / (ethylene + propylene + 1-butene) molar ratio shown in Table 1, the ethylene concentration at the ethylene / (ethylene + propylene + 1-butene) molar ratio shown in Table 1, and the 1-butene concentration at the 1-butene / (ethylene + propylene + 1-butene) molar ratio shown in Table 1.
[0122] The reaction heat (polymerization heat) was removed by the heat of vaporization of the liquefied propylene raw material supplied from pipe 3. Unreacted gas discharged from the polymerizer was cooled and condensed outside the reactor system through pipe 4 and then recirculated to polymerizer 5 through pipe 3. The generated polymer was continuously withdrawn from the polymerizer 5 through piping 6 so that the polymer retention level was 50% of the reaction volume. At this time, a portion of the polymer was intermittently sampled from pipe 6. The propylene-ethylene-1-butene copolymer was then used as a sample for measuring MFR, ethylene content, and 1-butene content after removing unreacted monomers. The production rate of the propylene-ethylene-1-butene copolymer was 10 kg / h, and the catalytic activity of the propylene polymerization catalyst, determined from the catalyst feed rate per hour (0.14 g / h) and the production rate (10 kg / h), was approximately 79,000 g / g-catalyst. The production conditions, monomer content, and various physical properties of propylene polymer-1 are shown in Table 1.
[0123] Manufacturing Example 2: Production of Propylene Polymer-2 Except for changing the catalyst feed amount, hydrogen concentration, ethylene concentration, and 1-butene concentration to the conditions shown in Table 1, the process was carried out under the same conditions as in Production Example 1 to obtain propylene polymer-2. The production conditions, monomer content, and various properties of propylene polymer-2 are shown in Table 1.
[0124] [Table 1]
[0125] [Propylene polymers (C) and (E)] Propylene-based polymers-1 and 2 obtained in Production Examples 1 and 2 were used.
[0126] [Propylene-based thermoplastic elastomers (D) and (F)] Propylene-based thermoplastic elastomer-1; manufactured by ExxonMobil, trade name: Vistamaxx (registered trademark) VM6102 [propylene-ethylene copolymer] MFR = 3.0 g / 10 min, Tm = 108°C, ΔHm = 7 J / g, flexural modulus = 11 MPa, density = 0.862 g / cm³ 3 Propylene content = 84% by weight, Ethylene content = 16% by weight
[0127] [Propylene homopolymer] Propylene homopolymer-1; Manufactured by Nippon Polypropylene Co., Ltd., Product name: Novatec® FL203D [Propylene homopolymer catalyzed by Ziegler-Natta catalyst] MFR = 3.0 g / 10 min, Tm = 162°C, ΔHm = 107 J / g, flexural modulus = 1,400 MPa, HDD = 80, Young's modulus (MD) = 760 MPa, density = 0.905 g / cm³ 3
[0128] [Other ingredients] Linear low-density polyethylene-1; manufactured by Nippon Polyethylene Co., Ltd., product name: Harmolex (registered trademark) NC564A MFR = 3.5 g / 10 min, Tm = 124°C, ΔHm = 124 J / g, flexural modulus = 160 MPa, HDD = 53, Young's modulus (MD) = 141 MPa, density = 0.918 g / cm³ 3
[0129] Example 1 1. Fabrication of a laminate of a base layer and an intermediate layer A 100% by weight pellet of propylene homopolymer-1 was used as the base layer, and a 100% by weight pellet of propylene-based polymer-1 was used as the intermediate layer. Using an extruder, the base layer was co-extruded at a resin temperature of 230°C and a width of 300 mm to obtain a laminate of the base layer and intermediate layer, with a thickness of 920 μm for the base layer and 80 μm for the intermediate layer. The obtained laminate was biaxially stretched using a JPP tenter (a biaxial stretching machine manufactured by Mitsubishi Heavy Industries, Ltd.) at a chill roll speed of 3 m / min, longitudinal and transverse stretching speeds of 15 m / min, longitudinal stretching ratio of 5x, and transverse stretching ratio of 8x. The intermediate layer of the obtained stretched film was corona-treated with a voltage of 0.6 kV to obtain a biaxially oriented polypropylene film consisting of a base layer and an intermediate layer. The biaxially oriented polypropylene film had a base layer thickness of 23 μm and an intermediate layer thickness of 2 μm.
[0130] 2. Preparation of sealant film 100 parts by weight of propylene polymer-2 (75 parts by weight) and propylene thermoplastic elastomer-1 (25 parts by weight) were mixed in a blender and then melt-extruded at 230°C to form pellets. The resulting pellets were melt-extruded from a T-die mounted on a 35mm diameter extruder at a resin temperature of 240°C and a width of 320mm to form a film. After corona treatment was applied to one side, an unstretched sealant film with a thickness of 50μm was produced. This was used as a heat seal layer.
[0131] 3. Fabrication of laminated film A solution of a urethane-based adhesive (manufactured by Sanyo Chemical Industries, Ltd., Eunoflex® J-24) and a diluent (manufactured by Toyo Ink Co., Ltd., NC401 Solvent C) mixed in a 1:1 ratio was applied to the corona-treated surface of the biaxially oriented polypropylene film by dry lamination, dried to form an adhesive layer, and then bonded to the corona-treated surface of a sealant film to obtain a laminated film. For the laminated film, the maximum heat seal strength, heat seal initiation temperature, resistance to bag drop at low temperatures, film thickness, haze, puncture strength, and recyclability were evaluated. The composition and evaluation results of the laminated film in Example 1 are shown in Table 2.
[0132] Example 2 A laminated film was obtained in the same manner as in Example 1, except that a pellet of 100% by weight of propylene polymer-2 was used as the intermediate layer. The composition and evaluation results of the laminated film of Example 2 are shown in Table 2.
[0133] Example 3 A laminated film was obtained in the same manner as in Example 1, except that as the intermediate layer, 75% by weight of propylene polymer-2 and 25% by weight of propylene thermoplastic elastomer-1 were thoroughly mixed in a blender and then melt-extruded at 230°C to form pellets. The composition and evaluation results of the laminated film of Example 3 are shown in Table 2.
[0134] Example 4 A laminated film was obtained in the same manner as in Example 3, except that 100% by weight pellets of propylene polymer-2 were used as the heat-seal layer. The composition and evaluation results of the laminated film of Example 4 are shown in Table 2.
[0135] Comparative Example 1 A laminated film was obtained in the same manner as in Example 1, except that a pellet of 100% by weight of propylene homopolymer-1 was used as the intermediate layer. The composition and evaluation results of the laminated film of Comparative Example 1 are shown in Table 2.
[0136] Comparative Example 2 A laminated film was obtained in the same manner as in Example 4, except that a pellet of 100% by weight of propylene homopolymer-1 was used as the intermediate layer. The composition and evaluation results of the laminated film of Comparative Example 2 are shown in Table 2.
[0137] Comparative Example 3 A laminated film was obtained in the same manner as in Comparative Example 1, except that 100% by weight of linear low-density polyethylene-1 pellets were used as the heat-seal layer. The composition and evaluation results of the laminated film of Comparative Example 3 are shown in Table 2.
[0138] Comparative Example 4 A laminated film was obtained in the same manner as in Example 4, except that E5102 (biaxially oriented polyethylene terephthalate film, 25 μm thick) manufactured by Toyobo Co., Ltd. was used instead of the biaxially oriented polypropylene film consisting of a base layer and an intermediate layer. The composition and evaluation results of the laminated film of Comparative Example 4 are shown in Table 2.
[0139] Comparative Example 5 A laminated film was obtained in the same manner as in Example 1, except that E5102 (biaxially oriented polyethylene terephthalate film, 25 μm thick) manufactured by Toyobo Co., Ltd. was used instead of the biaxially oriented polypropylene film consisting of a base layer and an intermediate layer. The composition and evaluation results of the laminated film of Comparative Example 5 are shown in Table 2.
[0140] Comparative Example 6 A laminated film was obtained in the same manner as in Comparative Example 3, except that E5102 (biaxially oriented polyethylene terephthalate film, 25 μm thick) manufactured by Toyobo Co., Ltd. was used instead of the biaxially oriented polypropylene film consisting of a base layer and an intermediate layer. The composition and evaluation results of the laminated film of Comparative Example 6 are shown in Table 2.
[0141] [Table 2]
[0142] As is clear from Table 1, the laminated films of Examples 1 to 4 had a heat seal initiation temperature of 140°C or lower, exhibiting excellent low-temperature heat sealability, a high maximum heat seal strength of 40 N / 15 mm or more, and excellent recyclability. In particular, Examples 1 to 3, in which the resin composition (B) constituting the heat seal layer has a propylene polymer (E) content of 50 to 95% by weight and a propylene thermoplastic elastomer (F) content of 5 to 50% by weight, are preferred because they exhibit excellent low-temperature heat sealability and maximum heat seal strength, as well as resistance to bag drop at low temperatures.
[0143] On the other hand, Comparative Examples 1-3, in which the intermediate layer is a propylene homopolymer, and Comparative Example 4, in which a commercially available biaxially oriented polyethylene terephthalate film was used instead of a biaxially oriented polypropylene film, exhibited inferior maximum heat seal strength. Furthermore, Comparative Examples 3-6 were not monomaterials and therefore had poor recyclability. The laminated film of the present invention has a maximum heat seal strength equivalent to laminated films using biaxially oriented polyethylene terephthalate film as the base layer, such as Comparative Examples 5 and 6, while being a monomaterial, it has excellent recyclability and can be suitably used as a film for various packaging applications. [Industrial applicability]
[0144] The laminated film can be suitably used as a packaging film for general foods, frozen foods, heavy goods, and liquids. [Explanation of symbols]
[0145] 1: Catalyst component supply piping (piping) 2: Raw material mixed gas supply piping (circulation piping) 3: Raw material propylene, 1-butene supply piping (piping) 4: Piping for extracting unreacted gas (piping) 5: Polymerizer (horizontal polymerizer) 6: Downstream end of the reactor (piping)
Claims
1. A laminated film comprising a base layer, an intermediate layer, and a heat-seal layer laminated in this order, The base layer and intermediate layer are stretched polypropylene films, and the heat-seal layer is an unstretched polypropylene film. A laminated film having an intermediate layer thickness of 1 to 10 μm, wherein the resin composition (A) constituting the intermediate layer satisfies the following requirement (a1), the resin composition (B) constituting the heat seal layer satisfies the following requirements (b1) to (b3), the resin composition (B) contains a propylene polymer (E), and the propylene polymer (E) satisfies the following requirements (e1) to (e5). (a1) The durometer D hardness (HDD) measured in accordance with JIS K 7215:1986 is between 10 and 78. (b1) The durometer D hardness (HDD) measured in accordance with JIS K 7215:1986 is between 10 and 65. (b2) Its melting point is 110 to 140°C. (b3) The flexural modulus measured at a test speed of 2 mm / min in accordance with JIS K 7171:2022 is 10 to 900 MPa. (e1) The MFR measured in accordance with JIS K 7210-1:2014 (230°C, 2.16 kg load) is 1 to 50 g / 10 min. (e2) In accordance with JIS K 7171:2022, the bending modulus measured at a test speed of 2 mm / min is greater than 500 MPa and less than or equal to 1,100 MPa. (e3) The content of units derived from propylene is greater than 88.0% by weight and 89.2% by weight or less. (e4) The content of units derived from ethylene and α-olefins having 4 to 20 carbon atoms is 10.8% by weight or more and less than 12.0% by weight. (e5) Its melting point is 110 to 140°C.
2. The resin composition (B) further comprises a propylene-based thermoplastic elastomer (F), wherein the content of the propylene-based polymer (E) is 10 to 90% by weight and the content of the propylene-based thermoplastic elastomer (F) is 10 to 90% by weight, based on a total of 100% by weight of the propylene-based polymer (E) and the propylene-based thermoplastic elastomer (F). The laminated film according to claim 1, wherein the propylene-based thermoplastic elastomer (F) satisfies the following requirements (f1) to (f4). (f1) The MFR measured in accordance with JIS K 7210-1:2014 (230°C, 2.16 kg load) is 1 to 30 g / 10 min. (f2) The flexural modulus measured at a test speed of 2 mm / min in accordance with JIS K 7171:2022 is 5 to 200 MPa. (f3) The content of units derived from propylene is 60.0 to 92.0% by weight. (f4) The content of units derived from ethylene and α-olefins having 4 to 20 carbon atoms is 8.0 to 40.0% by weight.
Citation Information
Patent Citations
Sealant film for retort
JP1997150491A
Laminate
JP2020192696A
Polypropylene-based non-stretched film, packaging material and package
JP2023161210A
Packaging material and package