Antifouling paint composition

The antifouling paint composition with copolymer A and antifouling agent D addresses low solubility issues in low-temperature seawater, ensuring stable and long-lasting antifouling performance.

JP7948642B2Active Publication Date: 2026-11-11NITTO KASEI CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2024573038
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2023-01-26
Filing Date
2024-01-22
Publication Date
2026-11-11
Estimated Expiration
2044-01-22

AI Technical Summary

Technical Problem

Existing antifouling coatings made from polymers containing (meth)acrylic acid alkoxycarbonylmethyl ester groups exhibit low solubility and poor performance in low-temperature seawater, leading to inadequate long-term antifouling properties.

Method used

An antifouling paint composition comprising a copolymer A, made from specific monomers, and an antifouling agent D, which maintains stable coating film dissolution and antifouling performance in low-temperature seawater.

Benefits of technology

The composition ensures stable coating film solubility and effective antifouling performance over an extended period, even in low-temperature conditions, preventing aquatic fouling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007948642000001
    Figure 0007948642000001
  • Figure 0007948642000002
    Figure 0007948642000002
  • Figure 0007948642000003
    Figure 0007948642000003
Patent Text Reader

Abstract

Provided is an antifouling coating composition capable of maintaining a stable coating film dissolution rate over a long period of time in low-temperature seawater and capable of maintaining stable antifouling performance. The present invention provides an antifouling coating composition containing a copolymer A and an antifouling agent D, wherein: the copolymer A is a copolymer of a monomer (a) represented by general formula (1) and an ethylenically unsaturated monomer (b) other than the monomer (a); monomer (a) is a compound in general formula (1) in which n is 2 or more; the monomer (b) contains a monomer (b1) represented by general formula (2); and the ratio of the monomer (b1) to the total of the monomer (a) and the monomer (b) is 0.01-2 mol%.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] This invention relates to an antifouling coating composition. [Background technology]

[0002] Aquatic fouling organisms such as barnacles, seldomegna, mussels, bryozoans, sea squirts, green laver, sea lettuce, and slime can attach to ships (especially the hulls), fishing nets, fishing net attachments, and underwater structures such as power plant water pipes, causing problems such as impaired functionality and damage to the appearance of these vessels. To prevent such problems, there are known technologies that involve applying an antifouling paint composition to ships and other vessels to form an antifouling coating, and then gradually releasing the antifouling agent from the coating to provide long-term antifouling performance (Patent Documents 1-4).

[0003] However, the antifouling coatings made of polymers containing (meth)acrylic acid alkoxycarbonylmethyl ester groups described in Patent Documents 1 to 4 have extremely low coating solubility, making it difficult for them to exhibit antifouling properties over a long period of time. To solve these problems, a technology has been proposed that enables coating solubility over a long period of time to exhibit antifouling performance (Patent Document 5). Furthermore, a technology has also been proposed that improves the physical properties of the coating, such as cracking and peeling (Patent Document 6). [Prior art documents] [Patent Documents]

[0004] [Patent Document 1] Special Publication No. 63-61989 [Patent Document 2] Japanese Patent Publication No. 2003-119420 [Patent Document 3] Japanese Patent Publication No. 2003-119419 [Patent Document 4] Japanese Patent Publication No. 2002-3776 [Patent Document 5] WO2020 / 045211 publication [Patent Document 6] WO2022 / 102492 publication [Overview of the project] [Problems that the invention aims to solve]

[0005] Although the antifouling coatings made from the antifouling coating compositions described in Patent Documents 5 and 6 have been improved in terms of coating film solubility and coating film physical properties, there is still room for improvement in coating film solubility in low-temperature sea areas such as below 15°C. Therefore, there has been a need for an antifouling coating composition that can maintain excellent antifouling performance over a long period of time even in low-temperature sea areas.

[0006] This invention has been made in view of these circumstances, and provides an antifouling coating composition that can maintain a stable coating film dissolution rate and stable antifouling performance over a long period of time in low-temperature seawater. [Means for solving the problem]

[0007] The present invention provides an antifouling paint composition containing copolymer A and an antifouling agent D, wherein copolymer A is a copolymer of monomer (a) represented by general formula (1) and ethylenically unsaturated monomer (b) other than monomer (a), monomer (a) includes a compound in general formula (1) in which n is 2 or more, monomer (b) includes monomer (b1) represented by general formula (2), and the ratio of monomer (b1) to the total of monomer (a) and monomer (b) is 0.01 to 2 mol%.

[0008] As a result of diligent research to solve the above problems, the inventors of the present invention have found that a composition containing copolymer A and antifouling agent D can solve the above problems, and have completed the present invention. [Modes for carrying out the invention]

[0009] The present invention will be described in detail below. In this specification, (meth)acrylic acid ester means acrylic acid ester or methacrylic acid ester, and (meth)acrylic acid means acrylic acid or methacrylic acid. 1. Antifouling paint composition The antifouling coating composition of the present invention contains copolymer A and antifouling agent D.

[0010] 1-1.Copolymer A Copolymer A is a copolymer of monomer (a) and an ethylenically unsaturated monomer monomer (b) other than monomer (a).

[0011] The content of monomer (a) relative to the total of monomer (a) and monomer (b) is preferably 10 to 90% by mass, and more preferably 20 to 70% by mass. Specifically, for example, these are 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, and 90% by mass, and may also be within the range of any two of the values ​​exemplified here. In this case, the coating film solubility is particularly good.

[0012] The content of monomer (b1) accounts for 0.01 to 2 molar mass% of the total molar mass of monomer (a) and monomer (b), and is more preferably 0.1 to 1 molar mass%. Specifically, for example, this could be 0.01, 0.05, 0.1, 0.5, 1.0, 1.5, or 2.0 mol%, and may be within the range of any two of the values ​​exemplified here.

[0013] 1-1-1. Monomer (a) Monomer (a) is represented by general formula (1).

[0014] [ka] (In the formula, R 1 R represents a hydrogen or methyl group. 2 R represents hydrogen, a methyl group, and a phenyl group. 3represents an alkyl group having 1 to 8 carbon atoms which may be substituted with an alkoxy group having 1 to 8 carbon atoms or a phenyl group, or represents a phenyl group, and n represents an integer of 1 to 10.)

[0015] R 2 is preferably hydrogen or a methyl group.

[0016] R 3 The alkyl group having 1 to 8 carbon atoms may or may not be substituted with a substituent. The substituent may be an alkoxy group having 1 to 8 carbon atoms or a phenyl group. R 3 The number of carbon atoms in the alkoxy group or alkyl group is, for example, 1, 2, 3, 4, 5, 6, 7, or 8, and may be in a range between any two of the exemplified numerical values herein. R 3 The alkyl group is, for example, a methyl group, ethyl group, n-propyl group, isopropyl group, n-butyl group, t-butyl group, 2-ethylhexyl group, cyclohexyl group, benzyl group, phenyl group, 2-methoxyethyl group, 4-methoxybutyl group, vinyl group, or allyl group, preferably a methyl group, ethyl group, isopropyl group, or n-butyl group.

[0017] n represents an integer of 1 to 10, and n is, for example, 1, 2, 3, 4, 5, 6, 7, 8, 9, or 10, and may be in a range between any two of the exemplified numerical values herein.

[0018] The monomer (a) includes a compound in which n in the general formula (1) is 2 or more. When the compound in which n is 2 or more is contained as the monomer (a), the coating film solubility is increased. The monomer (a) may be composed only of a compound in which n is 2 or more, or may be a mixture of a compound in which n is 1 and a compound in which n is 2 or more.

[0019] Monomer (a) is preferably composed of monomer (a1) and monomer (a2). The content of monomer (a1) in monomer (a) is preferably 50 to 80% by mass, more preferably 55 to 75% by mass, and particularly preferably 60 to 70% by mass. Compared to monomer (a2), monomer (a1) has the property of increasing the strength of the coating film and decreasing the solubility of the coating film. For this reason, if the content of monomer (a1) is too low, the strength of the coating film tends to be low, and the surface condition of the coating film may deteriorate after a long period of time. On the other hand, if the content of monomer (a1) is too high, the solubility of the coating film will be low, and the antifouling performance may decrease.

[0020] <Monomer (a1)> Monomer (a1) is a compound in which n in general formula (1) is 1. Examples of monomers (a1) include methoxycarbonylmethyl (meth)acrylate, ethoxycarbonylmethyl (meth)acrylate, isopropoxycarbonylmethyl (meth)acrylate, n-propoxycarbonylmethyl (meth)acrylate, n-butoxycarbonylmethyl (meth)acrylate, t-butoxycarbonylmethyl (meth)acrylate, 2-ethylhexyloxycarbonylmethyl (meth)acrylate, cyclohexyloxycarbonylmethyl (meth)acrylate, benzyloxycarbonylmethyl (meth)acrylate, phenoxycarbonylmethyl (meth)acrylate, 2-methoxyethoxycarbonylmethyl (meth)acrylate, 4-methoxybutoxycarbonylmethyl (meth)acrylate, allyloxycarbonylmethyl (meth)acrylate, vinyloxycarbonylmethyl (meth)acrylate, and 1-(methoxycarbonylmethyl (meth)acrylate. Examples include (meth)acrylate, 1-(ethoxycarbonyl)ethyl (meth)acrylate, 1-(n-propoxycarbonyl)ethyl (meth)acrylate, 1-(isopropoxycarbonyl)ethyl (meth)acrylate, 1-(n-butoxycarbonyl)ethyl (meth)acrylate, 1-(t-butoxycarbonyl)ethyl (meth)acrylate, α-(methoxycarbonyl)benzyl (meth)acrylate, and α-(ethoxycarbonyl)benzyl (meth)acrylate. Preferably, examples include methoxycarbonylmethyl (meth)acrylate, ethoxycarbonylmethyl (meth)acrylate, isopropoxycarbonylmethyl (meth)acrylate, n-propoxycarbonylmethyl (meth)acrylate, n-butoxycarbonylmethyl (meth)acrylate, 1-(methoxycarbonyl)ethyl (meth)acrylate, and 1-(ethoxycarbonyl)ethyl (meth)acrylate.

[0021] <Monomer (a2)> Monomer (a2) is a compound in which n in general formula (1) is 2 or greater. From the viewpoint of long-term antifouling properties, n in general formula (1) is preferably 2 to 6.

[0022] The monomer (a2) preferably contains both compounds where n is 2 and compounds where n is 3 or more. Specifically, for example, in terms of solid content, the mass ratio (n(2) / n(2~10)) is preferably 0.4 to 0.8, and more preferably 0.5 to 0.7. In this case, a tendency for stable coating film dissolution to be sustained has been observed. Specifically, this value is, for example, 0.40, 0.45, 0.50, 0.55, 0.60, 0.65, 0.70, 0.75, and 0.80, and may be within the range of any two of the values ​​exemplified here.

[0023] Examples of monomers (a2) include methyl (meth)acrylate di(oxycarbonylmethyl), ethyl (meth)acrylate di(oxycarbonylmethyl), isopropyl (meth)acrylate di(oxycarbonylmethyl), n-propyl (meth)acrylate di(oxycarbonylmethyl), n-butyl (meth)acrylate di(oxycarbonylmethyl), t-butyl (meth)acrylate di(oxycarbonylmethyl), 2-ethylhexyl (meth)acrylate di(oxycarbonylmethyl), and cyclohexyl (meth)acrylate di(oxycarbonyl) (Vonylmethyl), (meth)acrylate benzyl di(oxycarbonylmethyl), (meth)acrylate phenyl di(oxycarbonylmethyl), (meth)acrylate 2-methoxyethyl di(oxycarbonylmethyl), (meth)acrylate 4-methoxybutyl di(oxycarbonylmethyl), (meth)acrylate allyl di(oxycarbonylmethyl), (meth)acrylate vinyl di(oxycarbonylmethyl), (meth)acrylate methyl di[1-(oxypolycarbonyl)ethyl], (meth)acrylate ethyl di[1-(oxypolycarbonyl Examples include (meth)acrylate (1-(oxypolycarbonyl)ethyl), n-propyl di(meth)acrylate (1-(oxypolycarbonyl)ethyl), isopropyl di(meth)acrylate (1-(oxypolycarbonyl)ethyl), n-butyl di(meth)acrylate (1-(oxypolycarbonyl)ethyl), t-butyl di(meth)acrylate (1-(oxypolycarbonyl)ethyl), methyl di(meth)acrylate (α-(oxycarbonyl)benzyl), and ethyl di(meth)acrylate (α-(oxycarbonyl)benzyl), preferably methyl di(meth)acrylate (oxycarbonyl (methyl), (meth)acrylate ethyl di(oxycarbonylmethyl), (meth)acrylate di(oxycarbonylmethyl), (meth)acrylate n-propyl di(oxycarbonylmethyl), (meth)acrylate n-butyl di(oxycarbonylmethyl), (meth)acrylate di[1-(oxypolycarbonylethyl)], (meth)acrylate di[1-(oxypolycarbonylethyl)], (meth)acrylate poly(oxycarbonylmethyl), (meth)acrylate poly(oxycarbonylmethyl),(meth)Isopropyl poly(oxycarbonylmethyl) acrylate, (meth)n-propyl poly(oxycarbonylmethyl) acrylate, (meth)n-butyl poly(oxycarbonylmethyl) acrylate, (meth)t-butyl poly(oxycarbonylmethyl) acrylate, (meth)2-ethylhexyl poly(oxycarbonylmethyl) acrylate, (meth)cyclohexyl poly(oxycarbonylmethyl) acrylate, (meth)benzyl poly(oxycarbonylmethyl) acrylate, (meth)phenyl poly(oxycarbonylmethyl) acrylate, (meth)2-methoxyethyl poly(oxycarbonylmethyl) acrylate, (meth)4-methoxybutyl poly(oxycarbonylmethyl) acrylate, (meth)allyl poly(oxycarbonylmethyl) acrylate, (meth)vinyl poly(oxycarbonylmethyl) acrylate, (meth)methyl poly[1-(oxypolycarbonyl)ethyl] acrylate, (meth) Examples include n-propyl polyacrylate [1-(oxypolycarbonyl)ethyl], isopropyl polymethacrylate [1-(oxypolycarbonyl)ethyl], n-butyl polymethacrylate [1-(oxypolycarbonyl)ethyl], t-butyl polymethacrylate [1-(oxypolycarbonyl)ethyl], methyl polymethacrylate [α-(oxycarbonyl)benzyl], and ethyl polymethacrylate [α-(oxycarbonyl)benzyl], preferably ( Examples include methyl acrylate poly(oxycarbonylmethyl), ethyl methacrylate poly(oxycarbonylmethyl), isopropyl methacrylate poly(oxycarbonylmethyl), n-propyl methacrylate poly(oxycarbonylmethyl), n-butyl methacrylate poly(oxycarbonylmethyl), methyl methacrylate poly[1-(oxypolycarbonylethyl)], and ethyl methacrylate poly[1-(oxypolycarbonylethyl)].

[0024] 1-1-2. Monomers (b) Monomer (b) is an ethylenically unsaturated monomer other than monomer (a). Monomer (b) can be classified into monomer (b1) and monomer (b2), and the monomer (b) used for the polymerization of copolymer A at least includes monomer (b1).

[0025] The proportion of the monomer (b1) relative to the total of the monomer (a) and the monomer (b) is 0.01 to 2 mol%, preferably 0.1 to 1.5 mol%. Specifically, this proportion is, for example, 0.01, 0.05, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.5, 2.0 mol%, and may be a range between any two of the numerical values exemplified herein.

[0026] <Monomer (b1)> Monomer (b1) is one or two or more compounds selected from the compounds represented by general formula (2). [Chemical formula] (In the formula, R 4 represents hydrogen or a methyl group, R 5 represents hydrogen, a methyl group, or a phenyl group, and m represents an integer of 0 to 10.)

[0027] R 4 is preferably hydrogen. m is preferably 0 or 1, and more preferably 0. Specifically, m is, for example, 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, and may be a range between any two of the numerical values exemplified herein.

[0028] Examples of the monomer (b1) include (meth)acrylic acid and (meth)acrylic acid hydroxycarbonylmethyl.

[0029] <Monomer (b2)> Monomer (b2) is obtained by subtracting monomer (b1) from monomer (b). In other words, monomer (b2) is a monomer that cannot be represented by either general formula (1) or (2). Examples of monomer (b2) include (meth)acrylic acid esters, vinyl compounds, aromatic compounds, and dialkyl ester compounds of dibasic acids that cannot be represented by general formula (1) or (2).

[0030] Examples of monomer (b2) (meth)acrylic acid esters include methyl methacrylate, ethyl acrylate, ethyl methacrylate, butyl acrylate, butyl methacrylate, isobutyl acrylate, isobutyl methacrylate, t-butyl acrylate, t-butyl methacrylate, 2-ethylhexyl acrylate, 2-ethylhexyl methacrylate, lauryl acrylate, lauryl methacrylate, benzyl acrylate, benzyl methacrylate, phenyl acrylate, cyclic trimethylolpropaneformal acrylate, and other (meth)acrylic acid esters; Examples include silyl (meth)acrylate esters such as triisopropylsilyl acrylate and triisopropylsilyl methacrylate.

[0031] Examples of vinyl compounds that are monomers (b2) include vinyl chloride, vinylidene chloride, vinyl benzoate, vinyl butyrate, butyl vinyl ether, lauryl vinyl ether, and other vinyl compounds having functional groups.

[0032] Examples of monomeric aromatic compounds (b2) include styrene, vinyltoluene, and α-methylstyrene.

[0033] Examples of dialkyl ester compounds of dibasic acids, which are monomers (b2), include dibutyl maleate.

[0034] 1-1-3. Physical properties and manufacturing method of copolymer A The weight-average molecular weight (Mw) of copolymer A is preferably between 5,000 and 300,000. If the molecular weight is less than 5,000, the antifouling coating film becomes fragile and prone to peeling and cracking. If it exceeds 300,000, the viscosity of the polymer solution increases, making it difficult to handle. Specifically, Mw can be, for example, 5,000, 10,000, 20,000, 30,000, 40,000, 50,000, 60,000, 70,000, 80,000, 90,000, 100,000, 200,000, or 300,000, and may also be within the range of any two of the values ​​exemplified here.

[0035] One method for measuring Mw is gel permeation chromatography (GPC).

[0036] Copolymer A may be any of the following copolymers: a random copolymer, alternating copolymer, periodic copolymer, or block copolymer, with monomer (a1), monomer (a2), monomer (b1), and monomer (b2).

[0037] Copolymer A can be obtained, for example, by polymerizing monomer (a1), monomer (a2), monomer (b1), and monomer (b2) in the presence of a polymerization initiator.

[0038] Examples of polymerization initiators include azo compounds such as 2,2'-azobisisobutyronitrile, 2,2'-azobis(2-methylbutyronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), dimethyl-2,2'-azobisisobutyrate, dimethyl-2,2'-azobisisobutyrate, and 2,2'-azobis(N-butyl-2-methylpropionamide); benzoyl peroxide, di-tert-butyl peroxide, and tert-butyl peroxide. Cibenzoate, tert-butyl peroxyisopropyl carbonate, t-butyl peroxy-2-ethylhexanoate, t-hexyl peroxy-2-ethylhexanoate, di-t-hexyl peroxide, t-butyl peroxy-2-ethylhexyl monocarbonate, di-t-butyl peroxide, 1,1,3,3-tetramethylbutyl peroxyneodecanoate, t-amyl peroxyneodecanoate, t-hexyl peroxypivalate, Examples of polymerization initiators include peroxides such as t-amyl peroxypivalate and 1,1,3,3-tetramethylbutyl peroxy-2-ethylhexanoate. These polymerization initiators can be used individually or in combination of two or more. Particularly preferred polymerization initiators are 2,2'-azobisisobutyronitrile, 2,2'-azobis(2-methylbutyronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), dimethyl-2,2'-azobisisobutyrate, and 1,1,3,3-tetramethylbutyl peroxy-2-ethylhexanoate. The molecular weight of copolymer A can be adjusted by appropriately setting the amount of polymerization initiator used. In addition, a chain transfer agent can be used to adjust the molecular weight of the resulting polymer. Examples of chain transfer agents include mercaptans such as n-dodecyl mercaptan; thioglycolic acid esters such as octyl thioglycolate; α-methylstyrene dimer; and terpinolene.

[0039] Polymerization methods include, for example, solution polymerization, bulk polymerization, emulsion polymerization, suspension polymerization, and non-aqueous dispersion polymerization. Among these, solution polymerization or non-aqueous dispersion polymerization is particularly preferred because it allows for the simple and accurate acquisition of copolymer A.

[0040] In the polymerization reaction described above, an organic solvent may be used as needed. The organic solvent is not particularly limited, but examples include aromatic hydrocarbon solvents such as xylene and toluene; aliphatic hydrocarbon solvents; ester solvents such as ethyl acetate, butyl acetate, isobutyl acetate, methoxypropyl acetate, and propylene glycol 1-monomethyl ether 2-acetate; alcohol solvents such as isopropyl alcohol, butyl alcohol, and propylene glycol monomethyl ether; ether solvents such as dioxane, diethyl ether, and dibutyl ether; and ketone solvents such as methyl ethyl ketone and methyl isobutyl ketone. Among these, butyl acetate, isobutyl acetate, butyl alcohol, propylene glycol monomethyl ether, propylene glycol 1-monomethyl ether 2-acetate, toluene, and xylene are preferred. These solvents can be used individually or in combination of two or more. The reaction temperature in the polymerization reaction can be set appropriately depending on the type of polymerization initiator, etc., and is usually 50 to 160°C, preferably 60 to 150°C.

[0041] The polymerization reaction is preferably carried out under an inert gas atmosphere such as nitrogen gas or argon gas.

[0042] 1-2. Antifouling agent D Examples of antifouling agents D include inorganic agents and organic agents. Examples of inorganic agents include cuprous oxide, copper thiocyanate (generic name: copper rhodane), and copper powder. Of these, cuprous oxide and copper rhodane are particularly preferred, and cuprous oxide that has been surface-treated with glycerin, sucrose, stearic acid, lauric acid, lycithin, or mineral oil is even more preferred in terms of long-term stability during storage.

[0043] Examples of organic agents include 2-mercaptopyridine-N-oxide copper (generic name: copper pyrithione), 2-mercaptopyridine-N-oxide zinc (generic name: zinc pyrithione), zinc ethylene bisdithiocarbamate (generic name: zineb), 4,5-dichloro-2-n-octyl-3-isothiazolon (generic name: C9 211), 3,4-dichlorophenyl-NN-dimethylurea (generic name: diuron), 2-methylthio-4-t-butylamino-6-cyclopropylamino-s-triazine (generic name: irgarol 1051), 2-(p-chlorophenyl)-3-cyano-4-bromo-5-trifluoromethylpyrrole (generic name: Econea 28), and 4-[1-(2,3-dimethylphenyl)ethyl]-1H-imidazole (generic name: medetomidine). These antifouling agents can be used individually or in combination of two or more.

[0044] The content of antifouling agent D in the composition of the present invention is not particularly limited, but is usually 0.1 to 60.0% by mass on a solid content basis. The content of antifouling agent D may be, for example, 0.1, 0.5, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, or 60% by mass, and may be within the range of any two of the values ​​exemplified here.

[0045] 1-3. Other additives Furthermore, the resin for antifouling coatings of the present invention can be further modified as needed by adding resin components other than copolymer A, elution regulators, plasticizers, pigments, dyes, defoamers, dehydrators, thixotropes, organic solvents, etc., to produce an antifouling coating.

[0046] Examples of dissolution modifiers include monocarboxylic acids and their salts, such as rosin, rosin derivatives, naphthenic acid, cycloalkenylcarboxylic acid, bicycloalkenylcarboxylic acid, versatic acid, trimethylisobutenylcyclohexenecarboxylic acid, and their metal salts, or the aforementioned alicyclic hydrocarbon resins. These can be used individually or in combination of two or more. Examples of the rosin derivatives include hydrogenated rosin, disproportionated rosin, maleated rosin, formylated rosin, polymerized rosin, and the like. Examples of commercially available alicyclic hydrocarbon resins include Quinton 1500, 1525L, and 1700 (product names, manufactured by Nippon Zeon Co., Ltd.). Among these, rosin, rosin derivatives, naphthenic acid, versatic acid, trimethylisobutenylcyclohexenecarboxylic acid, or metal salts thereof are preferred.

[0047] Examples of dehydrating agents include calcium sulfate, synthetic zeolite-based adsorbents, orthoesters, silicates such as tetramethoxysilane and tetraethoxysilane, isocyanates, carbodiimides, and carbodiimidazoles. These can be used individually or in combination of two or more.

[0048] 2. Method for producing an antifouling paint composition The antifouling coating composition of the present invention can be produced, for example, by mixing and dispersing a mixture containing copolymer A, antifouling agent D, and other additives using a disperser. The aforementioned mixture is preferably a mixture in which various materials such as copolymer A and antifouling agent D are dissolved or dispersed in a solvent. As the aforementioned disperser, one that can be used as a fine grinder is preferably used. For example, commercially available homomixers, sand mills, bead mills, dispersers, etc. can be used. Alternatively, the mixture may be mixed and dispersed using a container equipped with a stirrer and containing glass beads for mixing and dispersion.

[0049] 3. Antifouling treatment method, antifouling coating, and painted product The antifouling treatment method of the present invention involves forming an antifouling coating film on the surface of an object to be coated using the above-mentioned antifouling coating composition. According to the antifouling treatment method of the present invention, the antifouling coating film gradually dissolves from the surface, and the coating film surface is constantly renewed, thereby preventing the adhesion of aquatic fouling organisms. Examples of objects to be coated include ships (especially the hulls), fishing gear, and underwater structures. The thickness of the antifouling coating should be set appropriately according to the type of object to be coated, the ship's cruising speed, seawater temperature, etc. For example, when the object to be coated is the bottom of a ship, the thickness of the antifouling coating is usually 50 to 700 μm, preferably 100 to 600 μm. [Examples]

[0050] The following examples illustrate the features of the present invention. However, the present invention is not limited to these examples. The weight-average molecular weight (Mw) is the value obtained by GPC (polystyrene equivalent). The GPC conditions are as follows: Device: HLC-8220GPC, manufactured by Tosoh Corporation. Column... TSKgel SuperHZM-M (2 pieces) Flow rate...0.35 mL / min Detector... RI Column constant temperature bath temperature: 40℃ Eluent...THF The heat residue was measured in accordance with JIS K 5601-1-2:1999 (ISO 3251:1993) "Test method for paint components - Heat residue".

[0051] 1. Manufacturing example 1-1. Example of monomer (a1) production <Manufacturing Example 1 (Manufacturing of Monomer a1-1)> In a four-necked flask equipped with a thermometer, condenser, stirrer, and dropping funnel, 109 g (1.00 mol) of methyl chloroacetate, 72 g (1.00 mol) of acrylic acid, 0.1 g of 4-methoxyphenol, and 500 g of ethyl acetate were charged. While stirring, 101 g (1.00 mol) of triethylamine was added dropwise, maintaining the temperature below 40°C. After the addition was complete, the mixture was stirred at 70-80°C for 6 hours. After the reaction was complete, the organic layer was washed with tap water, hydrochloric acid solution, and sodium bicarbonate solution in that order. The solvent was then removed by distillation under reduced pressure to obtain monomer a1-1: 129.7 g. <Manufacturing Examples 2-3 (Manufacturing of Monomers a1-2 to a1-3)> Monomers a1-2 to a1-3 were obtained by carrying out the reaction using the raw materials shown in Table 1 in the same procedure as in Production Example 1. The reaction conditions and yields for Production Examples 1 to 3 are shown in Table 1.

[0052] [Table 1]

[0053] 1-2. Example of monomer (a2) production <Manufacturing Example 4 (Manufacturing of Monomer a2-1)> (First reaction) In a four-necked flask equipped with a thermometer, condenser, and stirrer, 215 g (1.85 mol) of sodium monochloroacetate, 201 g (1.85 mol) of methyl chloroacetate, and 300 g of N-methyl-2-pyrrolidone were charged and stirred at 70-80°C for 6 hours. After the reaction was complete, 500 ml of toluene was added to the reaction solution, and the organic layer was washed with tap water, hydrochloric acid solution, and sodium bicarbonate solution in that order. The solvent was then removed by distillation under reduced pressure to obtain 262 g of methoxycarbonylmethyl chloroacetate.

[0054] (Second reaction) Next, in a four-necked flask equipped with a thermometer, condenser, stirrer, and dropping funnel, the products of the first reaction—methoxycarbonylmethyl chloroacetate: 200 g (1.20 mol), acrylic acid: 87 g (1.20 mol), 4-methoxyphenol: 0.1 g, and ethyl acetate: 500 g—were charged, and while stirring, triethylamine: 122 g (1.20 mol) was added dropwise while maintaining the temperature below 40°C. After the addition was complete, the mixture was stirred at 70-80°C for 6 hours. After the reaction was complete, the organic layer was washed with tap water, hydrochloric acid solution, and sodium bicarbonate solution in that order, and the solvent was removed by distillation under reduced pressure to obtain monomer a2-1: 230.6 g.

[0055] <Manufacturing Examples 5-18 (Manufacturing of Monomers a2-2 to a2-15)> By carrying out the reaction using the raw materials shown in Table 2 in the same procedure as in Production Example 4, monomers a2-2 to a2-15 shown in Table 2 were obtained. The reaction conditions and yields for Production Examples 4 to 18 are shown in Table 2.

[0056] [Table 2]

[0057] The details of the raw materials in Tables 1 and 2 are as follows: CAMe: Methyl chloroacetate CAEt: Ethyl Chloroethyl Acetate AA: Acrylic acid MAA: Methacrylic acid TEA: Triethylamine MEHQ: 4-Methoxyphenol CANa: Sodium monochloroacetate NMP:N-methyl-2-pyrrolidone

[0058] 1-3. Examples of copolymer solution preparation <Manufacturing Example P1 (Manufacturing of Copolymer Solution A-1)> In a four-necked flask equipped with a thermometer, condenser, stirrer, and dropping funnel, 50 g of xylene and 50 g of butyl acetate were charged as solvents, nitrogen gas was introduced, and the temperature was maintained at 88°C while stirring. To this, a mixture of monomers (a1), (a2), (b1), and (b2) in the amounts (g) shown in Table 3, and 2.0 g of 1,1,3,3-tetramethylbutyl peroxy-2-ethylhexanoate (initial addition) as a polymerization initiator was added dropwise over 3 hours while maintaining the temperature at 88°C. After stirring at 88°C for 1 hour, 0.1 g of 1,1,3,3-tetramethylbutyl peroxy-2-ethylhexanoate was added three times at 1-hour intervals, and the mixture was stirred at the same temperature for another 2 hours. The mixture was then cooled to room temperature to obtain copolymer solution A-1. The heating residue Mw of A-1 is shown in Table 3.

[0059] <Manufacturing Examples P2-P20 (Manufacturing of Copolymer Solutions A-2-17 and B-1-3)> Copolymer solutions A-2 to A-17 and B-1 to B-3 were obtained by carrying out the polymerization reaction in the same manner as in Production Example P1, except that the monomers, polymerization initiators, and solvents shown in Tables 3 to 5 were used. The heating residue and Mw of each polymer are shown in Tables 3 to 5. The units of the raw material amounts in the tables are grams. The percentage (mol%) of monomer (b1) in the tables was calculated by dividing the number of moles of monomer (b1) by the total number of moles of monomer (a) and monomer (b).

[0060] [Table 3]

[0061] [Table 4]

[0062] [Table 5]

[0063] 1-4. Other manufacturing examples <Manufacturing Example C1 (Manufacturing of Gum Rosin Solution)> A flask equipped with a thermometer, reflux condenser, and stirrer contained 300 g of Chinese gum rosin (WW) and 310 g of xylene. The flask was subjected to reflux dehydration under reduced pressure at 70-80°C for 1 hour to obtain a xylene solution of gum rosin (a brown, transparent liquid with 50% solids). The heating residue of the resulting solution was 50.3%.

[0064] <Manufacturing Example C2 (Manufacturing of Gumrosin Zinc Salt Solution)> In a flask equipped with a thermometer, reflux condenser, and stirrer, 240 g of Chinese gum rosin (WW) and 360 g of xylene were placed in the flask. Furthermore, 120 g of zinc oxide was added so that all the resin acid in the rosin would form a zinc salt. The mixture was then refluxed under reduced pressure at 70-80°C for 3 hours. After cooling and filtration, a xylene solution of gum rosin zinc salt (dark brown transparent liquid, 50% solids) was obtained. The heating residue of the obtained solution was 50.2%.

[0065] 2. Examples 1-17 and Comparative Examples 1-3 (Manufacturing of Paint Compositions) Paint compositions were prepared by mixing and dispersing the components shown in Tables 6 and 7 in the proportions (mass%) shown in the same tables with glass beads with a diameter of 1.5 to 2.5 mm.

[0066] [Table 6]

[0067] [Table 7]

[0068] The details of the ingredients in the table are as follows: <Anti-fouling agent> Cuprous oxide: Product name "NC-301" (manufactured by Nisshin Chemco Co., Ltd.) Copper pyrithione: Product name "Copper Omagine" (manufactured by LONZA Co., Ltd.)

[0069] <Dissolution modifier> Gum rosin solution: Use the solution prepared in manufacturing example C1. Gumrosin zinc solution: Use the solution prepared in manufacturing example C2.

[0070] <Pigments> Bengara: Product name "Bengara Kingyoku" (manufactured by Morishita Bengara Kogyo Co., Ltd.) Talc: Product name "Talc MS" (manufactured by Nippon Talc Co., Ltd.) Zinc oxide: Product name "Zinc Oxide Type 2" (manufactured by Seido Chemical Industry Co., Ltd.) Titanium dioxide: Product name "FR-41" (manufactured by Furukawa Machinery & Metal Co., Ltd.)

[0071] <Other additives> Disparon A603-20X: Amid-type thixotropic agent: Product name "Disparon A603-20X" (manufactured by Kusumoto Kasei Co., Ltd.) Tricresyl phosphate: (Manufactured by Daihachi Chemical Industry Co., Ltd.) Tetraethoxysilane: Trade name "Ethyl Silicate 28" (manufactured by Colcoat Co., Ltd.)

[0072] 3. Exam All paint compositions in the examples and comparative examples were placed in sealed containers within one hour of manufacture and left to stand for 30 days in a constant temperature chamber set at 50°C (accelerated degradation treatment) before use. The paints that underwent the aforementioned treatment were subjected to the following tests.

[0073] <Test Example 1 (Rotary Test)> A rotating drum with a diameter of 515 mm and a height of 440 mm was installed in the center of the tank and made motor-driven to rotate it. In addition, a cooling system to maintain a constant seawater temperature and an automatic pH controller to maintain a constant seawater pH were installed. The test plates were prepared according to the following method. First, a rust-preventive coating film was formed on a titanium plate (71 × 100 × 0.5 mm) by applying a rust-preventive paint (epoxy vinyl A / C) to a dry thickness of approximately 100 μm and allowing it to dry. Then, the paint compositions obtained in the examples and comparative examples were applied to a dry film thickness of approximately 450 μm and dried at 40°C for 3 days to prepare test plates. The fabricated test plate was fixed to the rotating drum of the above-mentioned device so that it was in contact with seawater, and the drum was rotated at a speed of 20 knots. During this time, the seawater temperature was maintained at 15°C and the pH at 8.0-8.2, and the seawater was replaced every two weeks. The initial thickness and the remaining film thickness of each test plate at 6 months after the start of the test were measured using a shape measuring laser microscope VK-X100 manufactured by Keyence Corporation. The amount of dissolved coating film per month (μm / month) was obtained by calculating the difference between these measurements, and the solubility of the coating film was evaluated. The evaluation results are shown in Tables 6 and 7.

[0074] In all comparative examples, the results were not favorable compared to the examples in terms of maintaining superior antifouling performance over a long period. To maintain superior antifouling performance over a long period, a coating dissolution rate of approximately 1.5 to 10 μm / month is required. However, in comparative examples 1 and 3, the coating dissolution rate was significantly low, and in comparative example 2, the paint gelled after the accelerated degradation treatment, making it impossible to conduct the target test.

Claims

[Claim 1] An antifouling paint composition containing copolymer A and antifouling agent D, The copolymer A is a copolymer of a monomer (a) represented by general formula (1) and an ethylenically unsaturated monomer (b) other than monomer (a). The monomer (a) includes a compound in which n in the general formula (1) is 2 or more. The monomer (b) includes monomer (b1) represented by general formula (2), An antifouling paint composition in which the ratio of monomer (b1) to the sum of monomer (a) and monomer (b) is 0.01 to 2 mol%. 【Chemistry 1】 (In the formula, R 1 R represents a hydrogen or methyl group. 2 R represents hydrogen, a methyl group, and a phenyl group. 3 (where n represents an integer from 1 to 10, and n represents an integer from 1 to 10.) 【Chemistry 2】 (In the formula, R 4 R represents a hydrogen or methyl group. 5 (where 'm' represents hydrogen, a methyl group, or a phenyl group, and 'm' represents an integer from 0 to 10.)

Citation Information

Patent Citations

  • Manufacture of composite coated tube for nuclear fuel

    JP1988061989A

  • Soil-preventing coating composition, soil-preventing coating film, base material coated with the coating film and method for preventing soil

    JP2002003776A

  • Antifouling coating material composition and coated article

    JP2003119419A

  • Antifouling coating material composition and coated article

    JP2003119420A

  • Biodegradable, thermally responsive injectable hydrogel for treatment of ischemic cardiomyopathy

    WO2015160793A1