Method for manufacturing polyamide resin film

By depolymerizing and polymerizing recycled polyamide resin waste to create a biaxially oriented film with controlled properties, the method addresses recycling challenges, enhancing film strength and printability while promoting environmental sustainability.

JP7948644B2Active Publication Date: 2026-11-11UNITIKA LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2025021342
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-01-24
Filing Date
2025-02-13
Publication Date
2026-11-11
Estimated Expiration
2041-01-22

AI Technical Summary

Technical Problem

Existing methods for recycling polyamide resin waste materials face challenges in producing films with high strength and printability due to increased foreign matter and thermal degradation, leading to reduced productivity and print defects, while laminated films are difficult to recycle effectively.

Method used

A method involving depolymerization of waste polyamide resin to monomers, followed by polymerization and scouring to produce a polyamide resin film, which includes adjusting moisture content and stretching to achieve a biaxially oriented film with controlled properties.

Benefits of technology

The method enables the production of polyamide resin films with improved printability and mechanical properties, allowing for higher recycling rates and environmental sustainability by utilizing recycled materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007948644000004
    Figure 0007948644000004
  • Figure 0007948644000001
    Figure 0007948644000001
  • Figure 0007948644000002
    Figure 0007948644000002
Patent Text Reader

Abstract

To provide a method for producing a polyamide resin film by using a polyamide resin obtained through polymerization of a regenerated monomer as a recycled material.SOLUTION: The method for producing a polyamide resin film comprises: (1) a step for generating a monomer from a depolymerization material (A); (2) a step for producing a polyamide resin (B) through polymerization using a material containing the monomer; (3) a step for refining the polyamide resin (B); and (4) a step for preparing an unstretched film by using a starting material containing the refined polyamide resin (B), and then stretching the unstretched film.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for producing a polyamide resin film containing a polyamide resin that uses a large amount of recycled raw materials.

Background Art

[0002] It has been a long time since environmental issues began to attract attention, and in recent years, awareness of ensuring environmental sustainability has been increasing anew. For a long time, there has been a high demand for recycling resin waste materials, and these are used as raw material resins. For example, waste materials generated during the production of stretched thermoplastic resin films include, in addition to waste scraps such as edge trimming scraps and slitting scraps, films that have not been commercialized as defective products. Material recycling is commonly performed, in which pellets produced by remelting these materials are used as remelted resin (raw material).

[0003] However, in material recycling, as the content of remelted resin increases, the content of foreign matter, thermally degraded products and the like increases, so polyamide resin films, which particularly have high stretching stress, are prone to breakage during stretching, leading to reduced productivity. Moreover, since it becomes difficult to control the amount of additives contained in the remelted resin, local characteristic changes also occur on the film surface, which may cause printing defects, adhesion failures and the like. As such, the amount of remelted resin that can be contained in a polyamide resin film is limited, and it is considered that there is a limit to increasing the recycling rate.

[0004] On the other hand, laminated films such as packaging films, in which multiple types of resin raw materials are laminated including a printing layer, a barrier layer, an adhesive layer, and a sealant layer, are difficult to separate into individual raw materials, and thus may be difficult to recycle in some cases.

[0005] In such cases, a method is known in which the resin waste material is depolymerized and used as a monomer (recycled monomer), and this is also called chemical recycling. In particular, various chemical recycling methods have been proposed for polyamide resins. For example, a method is known in which nylon 6 is melted, metals are removed, and ε-caprolactam obtained by the depolymerization reaction is recovered and used as a raw material for fibers, a raw material for resins, etc., and this recovered ε-caprolactam can be reused (Patent Documents 1 and 2). [Prior art documents] [Patent Documents]

[0006] [Patent Document 1] Japanese Patent Application Publication No. 7-330718 [Patent Document 2] China Publication Bulletin CN91106147.9 [Overview of the project] [Problems that the invention aims to solve]

[0007] However, even if monomers obtained by depolymerizing polyamide resin, which is a waste resin, are polymerized, a polyamide resin suitable for film cannot be obtained. In other words, it is not possible to obtain a film with excellent strength, elongation, etc.

[0008] Moreover, in recent years, a wide variety of printing has been applied to product packaging, such as packaging containers, and the demands on the appearance of the print are tending to increase, leaving room for improvement in the printability of film (especially the reproducibility of lighter areas (low-gradation areas) in the expression of shades).

[0009] Therefore, the main object of the present invention is to provide a method for producing a polyamide resin film using a polyamide resin obtained by polymerizing recycled monomers as a recycled raw material. Furthermore, the present invention aims to provide a polyamide resin film that exhibits printability and other properties equivalent to or better than conventional products. [Means for solving the problem]

[0010] In view of the problems of the prior art, the inventors conducted extensive research and, as a result, discovered that the above objective can be achieved by using a specific raw material containing recycled monomer in the manufacture of film, thus completing the present invention.

[0011] In other words, the present invention relates to the following polyamide resin and a method for producing the same. 1. A method for producing a polyamide resin film, (1) A step of producing monomers from depolymerization raw materials (A), (2) A step of producing a polyamide resin (B) by polymerizing a raw material containing the monomer, (3) Step of scouring the polyamide resin (B) (4) A process of preparing an unstretched film using a starting material containing refined polyamide resin (B), and then stretching the unstretched film. A method for producing a polyamide resin film, characterized by containing [the specified ingredient]. 2. The manufacturing method according to item 1, wherein the monomer comprises ε-caprolactam. 3. The manufacturing method according to item 1, further comprising a step of adjusting the moisture content of the unstretched film to 2 to 10% by mass prior to stretching. 4. The manufacturing method according to item 1, wherein the manufacturing method includes, as part of the starting material, a remelted resin obtained by melting a polyamide resin (excluding the polyamide resin (B)), and the content of the remelted resin is 1% by mass or more. 5. The manufacturing method according to item 1, wherein the relative viscosity ηR of the refined polyamide resin (B) is 2.5 to 4.5. 6. The manufacturing method according to item 1, wherein the depolymerizing raw material (A) is at least one of polyamide 6 resin and its oligomer. 7. 1000mm of the 10% gradation area of ​​the semitone print applied to the film. 2 A polyamide resin film with 100 or fewer dead pixels. 8. The polyamide resin film according to item 7, wherein the caprolactam monomer concentration in the polyamide resin film is 1.6% by mass or less. 9. The polyamide resin film according to item 7, wherein the content of amino-terminated groups and carboxyl-terminated groups in the polyamide resin film is 80 mmol / kg or less, each. 10. The polyamide resin film according to item 7, wherein the ratio of the minimum to maximum film impact strength (minimum / maximum) under a temperature of 23°C and a humidity of 50%RH is 0.5 to 1.0. 11. A polyamide resin film according to item 7, comprising a polyamide resin having a cooling crystallization peak with a full width at half maximum of 10°C or higher. 12. The polyamide resin film according to claim 7, which is biaxially oriented. 13. A laminated film comprising a polyamide resin film according to any one of items 7 to 12 above, and a sealant resin layer laminated on the polyamide resin film. 14. Packaging material comprising a polyamide resin film as described in any of items 7 to 12 above. 15. A polyamide resin film obtained by the manufacturing method described in any of the preceding paragraphs 1 to 6. [Effects of the Invention]

[0012] According to the present invention, even when using a polyamide resin obtained by polymerizing recycled monomers as a recycled raw material, it is possible to provide a polyamide resin film that exhibits printability and other properties equivalent to or better than conventional products (new products). More specifically, the present invention provides a polyamide resin film (particularly a biaxially oriented polyamide resin film) in which localized deterioration of print appearance and adhesion are effectively suppressed by using a polyamide resin made from recycled monomers.

[0013] Furthermore, the polyamide resin film of the present invention exhibits controlled variations in impact strength and excellent general physical properties such as film elongation, wettability, and haze, making it particularly suitable for use as a packaging material.

[0014] In the production method of the present invention, since waste resin materials can be used as raw materials, it is possible to provide a recycled polyamide resin film with a high recycling ratio of, for example, 50% or more. As a result, reuse of resources can be promoted, which can contribute to environmental conservation as a sustainable technology. [Brief Description of the Drawings]

[0015] [Figure 1] This is a diagram showing an outline of the method for evaluating the printability of the polyamide resin film of the present invention. [Mode for Carrying Out the Invention]

[0016] 1. Method for producing polyamide resin film The production method of the present invention is a method for producing a polyamide resin film, comprising: (1) a step of generating a monomer from the raw material for depolymerization (A) (depolymerization step), (2) a step of producing a polyamide resin (B) by polymerization using a raw material containing the aforementioned monomer (polymerization step), (3) a step of scouring the aforementioned polyamide resin (B) (scouring step) (4) a step of producing an unstretched film using a starting material containing the scoured polyamide resin (B), and then stretching the aforementioned unstretched film (film formation step) characterized by including

[0017] Depolymerization step In the depolymerization step, monomers are regenerated from the raw material for depolymerization (A) (hereinafter, such monomers are referred to as "regenerated monomers").

[0018] As the regenerated monomers, lactams are particularly preferred, and examples thereof include ε-caprolactam, enantholactam, capryllactam, lauryllactam and the like. Among these, ε-caprolactam is particularly more preferred.

[0019] The type of depolymerizing raw material (A) is not particularly limited, and various polyamide resins, as well as oligomers of various polyamide resins, can be used. More specifically, the various resins listed in polyamide resin (B) described later can be used as examples. Examples of oligomers include chain-like structures ranging from dimers to heptamers, and cyclic structures ranging from dimers to nocamers.

[0020] In particular, in the present invention, at least one of polyamide 6 resin and its oligomer can be suitably used as a depolymerization raw material (A). In particular, since polyamide 6 is a resin composed substantially of ε-caprolactam alone as monomer units, its ease of monomerization and purification / separation is also an advantage.

[0021] Polyamide resins can take various forms, including waste resin from switching between different grades during polymerization and from switching to the final product of film manufacturing, as well as waste materials such as trimming scraps and slitting scraps generated during film production, and defective films that were not commercialized. Using these materials as raw materials can contribute to the production of films with excellent printability and other properties, and also contribute to environmental protection through the utilization of waste materials.

[0022] Examples of oligomer forms include not only highly water-soluble oligomers recovered from the refining water generated during the refining of polyamide resin, but also residues after filtration that contain less water-soluble 2-8 mers.

[0023] The method for producing monomers from the depolymerization raw material (A) is not particularly limited as long as the desired monomer can be obtained, but preferably a depolymerization reaction of the depolymerization raw material (A) can be employed. That is, the depolymerization raw material (A) can be chemically decomposed by the depolymerization reaction to suitably obtain regenerated monomers.

[0024] The method and conditions for the depolymerization reaction are not particularly limited and can be carried out according to known methods. Therefore, for example, a catalyst may be used or not. It may also be carried out in the absence of water (dry reaction) or in the presence of water (wet reaction). Particularly from the viewpoint of productivity, a method of carrying out depolymerization in hot water vapor in the presence of a catalyst is preferred. Cyclic oligomers with low water solubility are difficult to depolymerize directly due to the slow hydrolysis rate of the amide bond, but by ring-opening polymerization to form chain molecules and then depolymerizing under the above conditions, recycled monomers can be suitably obtained from cyclic oligomers as well.

[0025] Polymerization process In the polymerization process, a polyamide resin (B) is produced by polymerization using a raw material containing the monomer (recycled monomer).

[0026] The above raw materials may consist entirely of recycled monomers, but it is preferable to use virgin monomers in combination. Here, virgin monomers are the opposite of recycled monomers and refer to monomers that have not undergone the depolymerization process of polymers. Commercially available virgin monomers can also be used. For example, commonly available monomers can be used as virgin monomers.

[0027] Recycled monomers may contain by-products that are difficult to separate. This can slightly reduce the crystallization rate of polyamide resins made from recycled monomers alone compared to polyamide resins made from virgin monomers alone, and further reduce the crystallization rate of polyamide resins polymerized using both recycled and virgin monomers. This crystallization rate is determined by the cooling crystallization temperature (T) of the obtained polyamide resin. CThe temperature was measured, and the full width at half maximum (FWHM) of the obtained crystallization peak was used as an indicator. In this invention, the FWHM is usually preferably 10°C or higher, more preferably 11°C or higher, and most preferably 12°C or higher. The wider the FWHM, the wider the range of crystallization rates, which makes it less likely for localized unevenness in the crystalline state of the film surface to occur as the film is stretched and crystallized, thereby improving uniformity and ultimately improving the printability of low-gradation areas. From this viewpoint, it is preferable to use a polyamide resin polymerized using a combination of recycled monomer and virgin monomer. The upper limit of the FWHM can be, for example, around 20°C, but is not limited thereto.

[0028] The recycled monomer content in the raw material is not particularly limited, but from the viewpoint of broadening the full width at half maximum, it is preferable to set the upper limit to 90% by mass or less, and more preferably to 80% by mass or less. The lower limit is not particularly limited, but from the viewpoint of increasing the recycling rate, it is preferable to set it to 5% by mass or more, and particularly preferably to 10% by mass or more.

[0029] In addition to recycled monomers, it is preferable to use virgin monomers in combination. In this case, the virgin monomer content in the raw materials is usually preferably about 10 to 95% by mass, and more preferably 20 to 90% by mass.

[0030] For example, it is possible to use ε-caprolactam (hereinafter referred to as "C-CL") regenerated by the depolymerization reaction of polyamide 6 resin in the monomer in a range of nearly 100% by mass, but it is preferable to include ε-caprolactam (hereinafter referred to as "V-CL") as a virgin monomer as a monomer other than C-CL.

[0031] Furthermore, the polyamide resin (B) may be end-capping as needed to suppress monomer formation during melting. For this reason, the raw materials may contain additives such as end-capping agents as needed. End-capping agents are not particularly limited and include, for example, organic glycidyl esters, dicarboxylic anhydrides, monocarboxylic acids such as benzoic acid, and diamines.

[0032] The polymerization method for obtaining polyamide resin (B) is not particularly limited, and known monomer polymerization methods can also be employed. For example, a method can be employed in which ε-caprolactam, water, and benzoic acid as a chelating agent are mixed, heated in a polymerization vessel, pressurized, and then polymerized under reduced pressure and dehydration until the desired viscosity is reached.

[0033] Scouring process In the refining process, the polyamide resin (B) is refined. This removes monomers contained in the polyamide resin, and the relative viscosity of the polyamide resin can be increased to a desired range, resulting in physical properties suitable for film formation.

[0034] The refining method is not limited, but it is particularly preferable to refining the polyamide resin (B) so that its relative viscosity (at 25°C) is in the range of approximately 2.5 to 4.5. Therefore, for example, it is preferable to refining the polyamide resin (B) using hot water at 90 to 100°C for about 15 to 30 hours.

[0035] The refining method itself can employ known methods such as immersing the polyamide resin (B) in hot water. In this case, the polyamide resin (B) can be refined in the form of a molded body, such as pellets.

[0036] The scouring process may be performed in a single step, but it may be carried out two or more times as needed. By thoroughly scouring, the monomers contained in the polyamide resin can be completely dissolved in hot water, thereby sufficiently reducing the monomer content in the polyamide resin after scouring.

[0037] The polyamide resin after the scouring process is preferably dried as needed. The drying conditions are not particularly limited. For example, hot air drying can be performed at around 100-130°C for 10-30 hours, but is not limited to this. More specifically, hot air drying can be performed at 110°C for 20 hours.

[0038] Film formation process In the film formation process, an unstretched film is prepared using a starting material containing refined polyamide resin (B), and then the unstretched film is stretched.

[0039] The aforementioned starting material only needs to contain polyamide resin (B), but may contain other components as needed. For example, in order to improve cost benefits, recycling rates, etc., it may contain remelted resin (D) obtained by melting polyamide resin (excluding polyamide resin (B)) to the extent that it does not hinder the effects of the present invention. In the present invention, as the remelted resin (D), from the standpoint of environmental protection and effective use of resources, resin waste of polyamide resin (especially polyamide 6 resin) can be suitably used. More specifically, examples include pellets formed by remelting unstretched scraps, edge trimming scraps, slitting scraps, defective products, etc., generated during the manufacture of polyamide resin film.

[0040] The content of remelted resin (D) in the starting material is not particularly limited, but from the viewpoint of increasing the recycling rate, it is preferably 1% by mass or more, and more preferably 5% by mass or more. On the other hand, the upper limit of the content of remelted resin (D) is usually 75% by mass or less, particularly preferably 65% ​​by mass or less, more preferably 50% by mass or less, and even more preferably 40% by mass or less, and most preferably 35% by mass or less. Remelted resin tends to have an increased amount of molecular chain ends and a decrease in viscosity, and its quality stability is also poor. If its content exceeds 75% by mass, in addition to a decrease in the relative viscosity as a film raw material, foreign matter, thermally degraded products, etc. increase, and problems such as breakage tend to occur during film formation. Also, the mechanical properties of the film tend to decrease, such as a decrease in tensile elongation. Furthermore, the content of oligomers such as caprolactam monomer and dimer generated in the stretching process increases, which can lead to problems such as a local decrease in printability in subsequent processes and an increase in the rate of bag breakage due to decreased adhesion, so there are concerns about the impact on practical performance.

[0041] Film scraps and defective products used as remeltable resin typically contain additives such as lubricants and antioxidants; however, the above content figures include the content of these additives.

[0042] Film scraps and defective products used as remeltable resin have varying concentrations of additives, such as lubricants and antioxidants, depending on the brand. Therefore, the higher the remeltable resin content in the polyamide resin film, the more localized the reduction in haze, surface wettability, printability, and adhesion of the resulting film may occur due to variations in the concentration distribution of the additives. For this reason, when a polyamide resin film is composed of multiple layers, the remeltable resin content in the surface layer (outermost layer) is preferably 50% by mass or less, more preferably 40% by mass or less, and most preferably 35% by mass or less.

[0043] On the other hand, in the intermediate layer (layers other than the outermost layer), a high remeltable resin content does not affect the film surface properties such as wettability and printability, so the remeltable resin content can be increased to increase the recycling rate. However, since this tends to increase film haze and worsen physical properties such as impact strength, it is preferable to keep the remeltable resin content in the intermediate layer at 75% by mass or less. The lower limit of the remeltable resin content in each layer can be, for example, around 5% by mass, but is not limited to this.

[0044] Other components included in the starting materials may include, for example, a polyamide resin (C) obtained by polymerization from a raw material consisting only of virgin monomers and not recycled monomers.

[0045] When a mixture of a polyamide resin (B) polymerized solely from recycled monomers and a polyamide resin (C) polymerized solely from virgin monomers as the starting material is used and melt-extruded, physical properties similar to those of a polyamide resin (B) polymerized using both recycled and virgin monomers can be obtained. However, from the viewpoint of obtaining more uniform film surface characteristics, it is preferable to polymerize using both recycled and virgin monomers. That is, a polyamide resin (B) composed of a polymer containing recycled and virgin monomers as monomer units can be suitably used.

[0046] The relative viscosity of each polyamide resin included in the starting material is not limited, but is particularly preferably between 2.5 and 4.5, and more preferably between 2.8 and 4.0. If a polyamide resin with a relative viscosity of less than 2.5 is used, film formation and stretching become difficult, and even if a polyamide resin film is obtained, its mechanical properties may be significantly reduced. Furthermore, if a polyamide resin with a relative viscosity exceeding 4.5 is used, the film formation properties may be impaired.

[0047] In this invention, the relative viscosity is the value measured using an Ubbelohde viscometer on a sample solution (at a temperature of 25°C) in which the resin to be measured is dissolved in 96% sulfuric acid to a concentration of 1.0 g / dl.

[0048] Furthermore, if necessary, one or more additives such as antioxidants, UV absorbers, preservatives, antistatic agents, antiblocking agents, and inorganic fine particles may be added to the starting material, to the extent that they do not adversely affect the performance of the film.

[0049] Furthermore, lubricants may be incorporated into the starting materials for purposes such as improving the slipperiness of the resulting film. Both inorganic and organic lubricants can be used. Specific examples of lubricants include clay, talc, calcium carbonate, zinc carbonate, wollastonite, silica, alumina, magnesium oxide, calcium silicate, sodium aluminate, calcium aluminate, magnesium aluminosilicate, glass balloons, carbon black, zinc oxide, antimony trioxide, zeolite, hydrotalcite, layered silicates, and ethylenebisstearamide. Among these, silica is particularly preferred. The lubricant content is not particularly limited, but a range of 0.01 to 0.3% by mass in the starting materials is appropriate.

[0050] The method for producing the unstretched film is not limited and can be formed by known film-forming methods. For example, it can be obtained by extruding the molten raw material from a T-die and then cooling it with a casting roll. In this case, it is necessary to accurately control the actual temperature of the casting roll surface in order to ensure uniform crystallinity of the unstretched film.

[0051] In this invention, it is preferable to adjust the moisture content of the unstretched film to about 2 to 10% by mass (particularly 4 to 8% by mass) as a moisture adjustment step, if necessary, before stretching. If the moisture content is lower than 2% by mass, the stretching stress increases, making it easy for problems such as film tearing to occur. If the moisture content is higher than 10% by mass, the thickness variation of the unstretched film becomes larger, and the thickness variation of the resulting stretched film also becomes larger.

[0052] In the moisture adjustment process, if the moisture content of the film is low (especially less than 2% by mass), the moisture content of the film is adjusted by passing the film through a moisture adjustment tank at a temperature of 40-90°C, more preferably 50-80°C, and adjusting the passing time. Pure water is usually used in the moisture adjustment tank, but if necessary, dyes, surfactants, plasticizers, etc. may be included in the treatment solution. Alternatively, moisture may be adjusted by spraying water vapor. On the other hand, if the moisture content of the film is high (especially more than 10% by mass), the moisture content of the film may be adjusted by passing the film through a drying oven and adjusting the passing time.

[0053] Next, the unstretched film is stretched. The stretching method is not particularly limited, and any stretching method can be used. In particular, biaxial stretching is preferred from the viewpoint of obtaining a film with excellent tensile elongation in both the MD and TD directions.

[0054] The biaxial stretching method is not limited to any specific method; for example, simultaneous biaxial stretching and sequential biaxial stretching can be used. For example, simultaneous biaxial stretching is preferred from the viewpoint of surface balance, minimizing the difference between tensile elongation, elastic modulus, and tensile strength in the MD and TD directions, while sequential biaxial stretching is preferred in terms of improving puncture strength and impact strength. These stretching methods can be appropriately selected depending on the desired film properties, application, etc.

[0055] The stretching ratio can be set appropriately according to the application, desired physical properties, etc., and can be, for example, 2 to 4 times in the MD direction and 2 to 4 times in the TD direction, but is not limited to this. The stretching temperature is also not limited and can be carried out within the range of, for example, 40 to 220°C. In particular, in the case of sequential stretching, it is preferable to stretch in the MD direction at 40 to 80°C and in the TD direction at 80 to 150°C. In the case of simultaneous biaxial stretching, it is preferable to stretch at 160 to 220°C.

[0056] The resulting biaxially oriented film is preferably subjected to a short heat treatment at a temperature of approximately 150-220°C, if necessary, in order to improve dimensional stability and suppress the rate of hot water shrinkage.

[0057] Furthermore, the polyamide resin film of the present invention may be subjected to surface treatments such as corona discharge treatment or easy-adhesion treatment, to the extent that it does not impair the effects of the present invention. In addition, for example, an easy-adhesion layer, a barrier coat layer, a printed layer, etc., may be provided as needed.

[0058] The polyamide resin film obtained in this manner can also be provided as a laminate in which other layers are laminated together as needed.

[0059] Furthermore, during the manufacturing process of the polyamide resin film, a film composed of multiple layers may be formed by co-melt extrusion, lamination, or the like. For example, a two-layer configuration may be used, where a polyamide resin film containing a polyamide 6 resin polymerized from recycled monomers is laminated with a polyamide 6 resin film containing a remeltable resin. Alternatively, a three-layer configuration may be used, where a polyamide 6 resin film containing a remeltable resin is sandwiched between two polyamide resin films containing a polyamide 6 resin polymerized from recycled monomers. With a polyamide 6 resin film having a layer configuration that allows for the sandwiching of intermediate layers, such as a three-layer configuration, the remeltable resin content of the intermediate layer can be increased.

[0060] 2. Polyamide resin film This invention relates to a 1000mm semitone print applied to a film with a 10% gradation. 2This includes polyamide resin films characterized by having 100 or fewer dead pixels.

[0061] (1) Composition of polyamide resin film The composition of the polyamide resin is not particularly limited, and examples include polyamide 6 resins using lactams such as ε-caprolactam as monomers. Other examples of polyamide resins include those obtained by polycondensation of lactams with three or more membered rings, ω-amino acids, dibasic acids, diamines, etc.

[0062] More specifically, examples of lactams include ε-caprolactam, as mentioned earlier, as well as enantractams, capryllactams, lauryllactams, and others.

[0063] Examples of ω-amino acids include 6-aminocaproic acid, 7-aminoheptanoic acid, 9-aminononanoic acid, and 11-aminoundecanoic acid.

[0064] Examples of dibasic acids include adipic acid, glutaric acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, undecandionic acid, dodecadionic acid, hexadecadionic acid, eicosanedionic acid, eicosadienedionic acid, 2,2,4-trimethyladipic acid, terephthalic acid, isophthalic acid, 2,6-naphthalenedicarboxylic acid, xylylenedicarboxylic acid, and the like.

[0065] Examples of diamines include ethylenediamine, trimethylenediamine, tetramethylenediamine, hexamethylenediamine, pentamethylenediamine, undecamethylenediamine, 2,2,4 (or 2,4,4)-trimethylhexamethylenediamine, cyclohexanediamine, bis-(4,4′-aminocyclohexyl)methane, metaxylylenediamine, nonanediamine, and decanediamine.

[0066] Polymers or copolymers thereof obtained by polycondensation of these include, for example, polyamides 6, 7, 10, 11, 12, 4, 10, 5.6, 6.6, 6.9, 6.10, 6.11, 6.12, 10.10, 6T, 9T, 10T, 6I, MXD6 (metoxylendipanamide 6), 6 / 6.6, 6 / 12, 6 / 6T, 6 / 6I, 6 / MXD6, etc. Among these, polyamide 6 resin is preferred in the present invention because it has an excellent balance between heat resistance and mechanical properties. In other words, polyamide 6 resin film is preferred as the polyamide resin film of the present invention.

[0067] (2) Physical properties of polyamide resin film The polyamide resin film of the present invention has a 1000 mm semitone print applied to the film, with a 10% gradation area. 2 The film has printability with 100 or fewer dead pixels. Films with such characteristics are advantageous when printing in terms of high reproducibility in the printed appearance, especially in the lighter areas of the print. The number of dead pixels is preferably 80 or less, more preferably 70 or less, and most preferably 60 or less. If the number exceeds 100, unevenness can be seen with the naked eye, even in the low-gradation areas, and individual differences in the design can be perceived, potentially leading to the judgment of a printing defect. The lower limit of the number of dead pixels is most preferably 0, but it may be around 30, for example, but is not limited to this.

[0068] The polyamide resin film of the present invention preferably has a relative viscosity ηR of 2.5 to 4.5, and more preferably in the range of 2.8 to 4.0. The relative viscosity in this invention is measured using an Ubbelohde viscometer on a sample solution (at a liquid temperature of 25°C) prepared by dissolving the film to be measured in 96% sulfuric acid to a concentration of 1.0 g / dl. Polyamide resin films with a relative viscosity of less than 2.5 may exhibit significantly reduced mechanical properties or a lower evaluation in the drop bag test of the laminated film described later. Furthermore, polyamide resin films with a relative viscosity exceeding 4.5 tend to have insufficient uniformity of film thickness, which may result in uneven mechanical properties.

[0069] The polyamide resin film of the present invention preferably has a thickness accuracy of within plus or minus 15% of the target thickness, and more preferably within plus or minus 10%.

[0070] The polyamide resin film of the present invention preferably has an extract amount of caprolactam monomer of 1.6% by mass or less, more preferably 1.0% by mass or less, even more preferably 0.5% by mass or less, and most preferably 0.1% by mass or less. If the extract amount of caprolactam monomer exceeds 1.6% by mass, the wettability of the surface of the polyamide resin film tends to vary. In addition, the adhesion between the polyamide resin film and other resin layers or inks may decrease locally, which may result in a decrease in practical performance, such as in the bag drop test, where the number of times until the bag breaks.

[0071] The polyamide resin film of the present invention preferably contains 80 mmol / kg or less of amino-terminated groups and carboxyl-terminated groups, and most preferably contains 70 mmol / kg or less of each. If the content of amino-terminated groups and carboxyl-terminated groups exceeds 80 mmol / kg, the crystallization rate of the film increases, and localized variations in crystallinity tend to occur. This can lead to a decrease in the localized printability of the film, as well as a decrease in tensile elongation, and variations in physical properties such as impact strength, sometimes resulting in partial declines.

[0072] The polyamide resin film of the present invention preferably has a ratio (minimum / maximum) of 0.5 to 1.0 between the minimum and maximum impact strength of the film under a temperature of 23°C and a humidity of 50% RH, more preferably between 0.6 and 1.0, and most preferably between 0.7 and 1.0. If the ratio is less than 0.5, it is considered that there is a partial decrease in the impact resistance of the film, which is not practically desirable.

[0073] The polyamide resin film of the present invention preferably has a tensile elongation of 60% or more in both the MD and TD directions, and more preferably 70% or more.

[0074] The polyamide resin film of the present invention preferably has a haze value of 10.0% or less, more preferably 7.0% or less, and most preferably 6.0% or less.

[0075] The polyamide resin film of the present invention is preferably a film obtained by the method described in "1. Method for producing a polyamide resin film" above. That is, it is preferable that the film be produced using raw materials containing recycled monomers. Therefore, the polyamide resin film of the present invention is preferably a stretched film (particularly a biaxially stretched film). This makes it possible to more reliably obtain the above-mentioned physical properties.

[0076] Therefore, the polyamide resin film of the present invention may consist solely of a polyamide resin film polymerized from recycled monomers, a mixture of two or more types, or a polyamide resin film containing a remeltable resin as described later. It may also consist of a single layer, or it may be a film composed of multiple layers formed by simultaneous melt extrusion or lamination. For example, it may be a two-layer configuration in which a polyamide resin film containing a polyamide resin polymerized from recycled monomers is laminated with a polyamide resin film containing a remeltable resin, or a three-layer configuration in which a polyamide resin film containing a remeltable resin is sandwiched between polyamide resin films containing a polyamide resin polymerized from recycled monomers. When composed of multiple layers, it is preferable that at least one of the outermost layers contains a polyamide resin polymerized from recycled monomers.

[0077] (3) Use of polyamide resin film The polyamide resin film (particularly the biaxially oriented polyamide resin film) obtained as described above possesses excellent mechanical properties such as tensile elongation, tensile strength, and elastic modulus as a polyamide resin film, as well as excellent transparency, color tone, wettability, and printability, making it particularly suitable for use as a packaging material.

[0078] The polyamide resin film of the present invention can be used alone or laminated with other layers to form a laminate. For example, an easy-adhesion layer, a barrier coating layer, a printed layer, an adhesive layer, etc., can be provided as needed.

[0079] The polyamide resin film of the present invention can be laminated with a sealant layer such as polyolefin using known methods such as dry lamination or extrusion lamination to form a laminated film, and the opposing sealant layers can be heat-sealed together to be used as a packaging bag (bag body). Any form of bag body can be used, such as two-side bags, three-side bags, gusseted bags, side-sealed bags, stand-up pouches, and stand-up zipper bags.

[0080] The packaging material is not limited to the contents and can be used in a wide range of applications, including food and beverages, pharmaceuticals, cosmetics, chemicals, and general merchandise.

[0081] The present invention also includes laminated films comprising the polyamide resin film of the present invention and a sealant resin layer laminated on the polyamide resin film. Such laminated films can also be suitably used as packaging materials or packaging bodies. The polyamide resin film of the present invention has a uniform surface condition, with little localized precipitation of additives or monomers, and does not cause localized deterioration of adhesion, so the resulting packaging bodies have excellent resistance to tearing. For example, when a water-filled packaging body is dropped and tears, it may tear from areas with low strength, as well as delaminate and tear from areas with localized low adhesion. In contrast, the laminated film of the present invention has the advantage of being less prone to tearing compared to conventional products.

[0082] More specifically, in a drop bag test conducted at 25°C and a 55% RH atmosphere, the laminated film of the present invention preferably takes 50 or more drops before bursting, more preferably 60 or more drops, and even more preferably 70 or more drops. The drop bag test is conducted by dropping a package (made by heat-sealing two 200mm x 300mm laminated sheets with a 10mm width) filled with 1000ml of water and 10ml of air from a height of 1.2m. [Examples]

[0083] Examples and comparative examples are shown below to more specifically describe the features of the present invention. However, the scope of the present invention is not limited to the examples.

[0084] 1. About the raw materials used The raw materials used in the examples and comparative examples are as follows. Table 1 shows the time required for the polymerization reaction and the total processing time for scouring for each raw material, as well as the relative viscosity (ηR), cooling crystallization temperature (Tc) and its full width at half maximum, and monomer content (caprolactam content) of the obtained raw materials.

[0085] Raw materials B2~B4 Resin waste (resin waste material) containing film scraps or defective products generated during the manufacture of polyamide 6 resin film, and oligomers etc. produced during the polymerization of polyamide 6 resin, was used as the depolymerization raw material (A). Phosphoric acid was added to the depolymerization raw material (A), and the depolymerization reaction was carried out under heating using a wet method. After purification by activated carbon treatment, concentration, and distillation, the regenerated ε-caprolactam "C-CL" was recovered. On the other hand, "V-CL" is ε-caprolactam, which is a virgin monomer. C-CL and V-CL were blended in the ratios (mass ratios) shown in Table 1. This mixture was then mixed with water and benzoic acid as a chelating agent. The mixture was heated, pressurized, depressurized, and dehydrated in a polymerization vessel, and then polymerized until the desired viscosity was achieved. The required polymerization time for the final desired viscosity varied depending on the ratio of CL species. The polymerization times for each type are shown in Table 1. After pelletizing the obtained polymer (resin), it was refined twice by hot water treatment at 95°C for 10 and 15 hours, and then dried at 110°C for 20 hours. In this way, polyamide resins (raw materials B2-4) with a relative viscosity of 3.1 were obtained.

[0086] Raw materials B1, B5 Using C-Cl, water, and benzoic acid as a chelating agent as raw materials, polymerization was carried out in the same manner as described above, followed by pelletization. The resulting material was then scouring twice with hot water at 95°C for 10 and 15 hours, and finally dried at 110°C for 20 hours. In this way, a polyamide resin (B1) with a relative viscosity of 3.0 was obtained. Furthermore, the polyamide resin (B1) was polymerized under the same conditions, pelletized, and then refined by hot water treatment at 95°C for 18 hours, followed by drying at 110°C for 20 hours. In this way, a polyamide resin (raw material B5) with a relative viscosity of 2.7 was obtained.

[0087] Raw material B6 The material was polymerized under the same conditions as raw material B1, pelletized, then refined by hot water treatment at 95°C for 10 hours, and dried at 110°C for 20 hours. In this way, a polyamide resin (raw material B6) with a relative viscosity of 2.4 was obtained.

[0088] Raw material C Using V-CL, water, and benzoic acid as a chelating agent as raw materials, polymerization was carried out in the same process, followed by pelletization. After being scouring twice by hot water treatment at 95°C for 10 hours each, the material was dried at 110°C for 20 hours. In this way, a polyamide resin (raw material C) with a relative viscosity of 3.1 was obtained.

[0089] Raw material D Film waste generated during the production of polyamide 6 resin film was crushed, remelted at 250-290°C, and then pelletized. Afterward, it was dried. In this way, remelted resin (raw material D) was obtained. The relative viscosity of the remelted resin was 2.9.

[0090] Silica Master E (Silica-containing polyamide resin, containing 6% silica by mass) A master chip manufactured by Ikegai Seisakusho, PCM-30, was used. A1030BRF (polyamide 6 resin manufactured by Unitika Corporation) / Silica 1 (Silysia 310P manufactured by Fuji Silysia Chemical Co., Ltd., average particle size 1.4 μm) / Silica 2 (Mizukasil P73 manufactured by Mizusawa Chemical Industry Co., Ltd., average particle size 2.5 μm) was fed in from the supply port in a ratio of 94.0 / 4.5 / 1.5 (mass ratio). The mixture was melted and kneaded under the conditions of cylinder temperature 230°C to 270°C, screw rotation speed 200 rpm, and discharge rate 10 kg / hour. The resulting molten mixture was pelletized and vacuum dried (80°C for 24 hours). Silica Master E was thus obtained. The relative viscosity of the silica master was 3.0.

[0091] [Table 1]

[0092] 2. Examples and Comparative Examples A film was prepared using each of the raw materials described in section 1 above.

[0093] Example 1 As the composition of the polyamide resin film, 97.5% by mass of polyamide resin (raw material B1) polymerized only of C-CL and 2.5% by mass of silica master were mixed and melt-kneaded in an extruder, supplied to a T-die and extruded in a sheet form, wound onto a metal drum heated to 20°C, cooled and then wound up to obtain an unstretched film with a thickness of approximately 150 μm. Next, the obtained unstretched film was immersed in a moisture-adjusting tank heated to 50°C for 1 minute, and then the ends were held with clips of a tenter-type simultaneous biaxial stretching apparatus and simultaneously biaxially stretched at a stretch ratio of 3.0 times in the MD direction and 3.3 times in the TD direction under conditions of 180°C. After that, a heat treatment was performed at 201°C for 4 seconds with a relaxation rate of 5% in the TD direction, then slowly cooled to room temperature, and corona discharge treatment was performed on one side. After that, the film was wound up to obtain a biaxially oriented polyamide resin film with a thickness of 15 μm. The total regeneration ratio in this film was 97.5% by mass. Furthermore, the moisture content of the unstretched film was 5% by mass.

[0094] Example 2 A biaxially oriented polyamide resin film with a thickness of 15 μm was obtained in the same manner as in Example 1, except that 97.5% by mass of the polyamide resin (raw material B5) shown in Table 1 was used as the composition of the polyamide resin film. The total recycled content in this film was 97.5% by mass.

[0095] Examples 3, 5, and 13 A biaxially oriented polyamide resin film with a thickness of 15 μm was obtained in the same manner as in Example 1, except that the polyamide resin (raw material B4), (raw material B3), or (raw material B2) listed in Table 1 was used in a composition of 97.5% each, as shown in Table 2. The total recycled content in this film was 87.8% by mass, 39.0% by mass, and 19.5% by mass, respectively.

[0096] Examples 4, 11, 18 A biaxially oriented polyamide resin film with a thickness of 15 μm was obtained in the same manner as in Example 1, except that the polyamide resin (raw material B1) and polyamide resin (raw material C) listed in Table 1 were blended in the ratios shown in Table 2, and 97.5% of this blended resin was used.

[0097] Examples 6, 7, 9, 10, 16, 17 A biaxially oriented polyamide resin film with a thickness of 15 μm was obtained in the same manner as in Example 1, except that the composition of the polyamide resin film was obtained by blending the polyamide resin (raw material B1) and polyamide resin (raw material C) listed in Table 1 with the remelted resin (raw material D) in the ratios shown in Table 2, and using 97.5% by mass of this resin.

[0098] Example 8 A biaxially oriented polyamide resin film with a thickness of 15 μm was obtained in the same manner as in Example 1, except that the polyamide resin (raw material B3) from Table 1 and the remelt resin (raw material D) were blended in the ratios shown in Table 2, and 97.5% by mass of this resin was used.

[0099] Examples 14 and 15 A biaxially oriented polyamide resin film with a thickness of 15 μm was obtained in the same manner as in Example 1, except that the polyamide resin (raw material B2) from Table 1 and the remelt resin (raw material D) were blended in the ratios shown in Table 2, and 97.5% by mass of this resin was used.

[0100] Example 12 For the composition of the polyamide resin film, the polyamide resin (raw material B1) and polyamide resin (raw material C) listed in Table 1 were blended in the ratios shown in Table 2. This resin was mixed with 97.5% by mass and silica master at 2.5% by mass to obtain an unstretched film in the same manner as in Example 1. Next, the unstretched film was stretched 2.8 times in the MD direction on a temperature-controlled roll at 55°C, then held with clips and stretched 3.7 times in the TD direction under conditions of 185°C (sequential biaxial stretching). Subsequently, a heat treatment was performed at 201°C for 4 seconds with a relaxation rate of 5% in the TD direction, and after slow cooling to room temperature, corona discharge treatment was performed on one side. The film was then wound up to obtain a biaxially oriented polyamide resin film with a thickness of 15 μm. The total regeneration rate in this film was 19.5% by mass. The moisture content of the unstretched film was 0.5% by mass.

[0101] Example 19 A polyamide resin film consisting of two types and three layers with a thickness ratio of 1:1:1 was fabricated. As the intermediate layer, a resin was arranged by mixing 25% by mass of polyamide resin (raw material C) from Table 1 and 75% by mass of remelted resin (raw material D). As the outer layers, polyamide resin (B3) from Table 1 was arranged. Except for mixing 2.5% by mass of silica master into each layer and co-extruding, an unstretched film was obtained in the same manner as in Example 1, and a biaxially oriented polyamide resin film with a thickness of 15 μm was obtained by simultaneous biaxial stretching. The total regeneration rate in this film was 50.4% by mass.

[0102] Comparative Example 1 A biaxially oriented polyamide resin film with a thickness of 15 μm was obtained in the same manner as in Example 1, except that 97.5% by mass of the polyamide resin (B6) shown in Table 1 was used as the composition of the polyamide resin film.

[0103] Comparative Example 2 A biaxially oriented polyamide resin film with a thickness of 15 μm was obtained in the same manner as in Example 1, except that 97.5% by mass of remelted resin (D) was used as the composition of the polyamide resin film.

[0104] Comparative Example 3 A biaxially oriented polyamide resin film with a thickness of 15 μm was obtained in the same manner as in Example 12, except that 97.5% by mass of remelted resin (D) was used as the composition of the polyamide resin film.

[0105] Comparative Examples 4 and 5 A biaxially oriented polyamide resin film with a thickness of 15 μm was obtained in the same manner as in Example 1, except that the composition of the polyamide resin film was obtained by blending polyamide resin (C) and remelt resin (D) in the ratios shown in Table 2, and using 97.5% by mass of this resin.

[0106] Comparative Example 6 A biaxially oriented polyamide resin film with a thickness of 15 μm was obtained in the same manner as in Example 1, except that 97.5% by mass of polyamide resin (C) was used as the composition of the polyamide resin film.

[0107] Comparative Example 7 As the composition of the polyamide resin film, 97.5% by mass of polyamide resin (C) and 2.5% by mass of master chip (E) were mixed and melt-kneaded in an extruder, supplied to a T-die and extruded in a sheet form, wound onto a metal drum heated to 20°C, cooled and then wound up to obtain an unstretched film with a thickness of approximately 150 μm. At this time, variations were observed in the actual temperature of the metal drum, which was heated to 20°C, and variations occurred in the crystallinity of the unstretched film. Except for this, a biaxially oriented polyamide resin film with a thickness of 15 μm was obtained in the same manner as in Example 1. The thickness accuracy of the obtained film was found to be greater than plus or minus 15% in some areas.

[0108] [Table 2]

[0109] Test Example 1 The following physical properties were investigated for the raw material polyamide resins (raw materials B1 to D) and the films obtained in each example and comparative example. The results are shown in Table 3. For each measurement, samples were left in an environment of 23°C and 50% RH for at least 2 hours, and measurements were taken in an atmosphere of 23°C and 50% RH.

[0110] (1) Relative viscosity ηR The raw material polyamide resins (raw materials B1 to D) and the films obtained in each example and comparative example were used as samples. The relative viscosity of the sample solutions (at a temperature of 25°C) prepared by dissolving them in 96% sulfuric acid to a concentration of 1.0 g / dl was measured using an Ubbelohde viscometer.

[0111] (2) Moisture content Unstretched film was collected after water absorption treatment or immediately before stretching, placed in a weighing bottle, dried, and the mass change before and after drying was used to calculate the mass.

[0112] (3) Caprolactam monomer content [Preparation of the measurement sample] The polyamide resin raw materials (raw materials B1-D) and the films obtained in each example and comparative example were freeze-dried and weighed to 0.5 g, placed in a 10 ml headspace bottle, 10 ml of ultrapure water was added, and the bottle was sealed with a butyl rubber stopper and an aluminum cap. Extraction was then carried out in a boiling water bath (100°C) for 2 hours. After cooling, the mixture was filtered through a 0.45 μm disc filter to obtain the measurement sample. [Creating a calibration curve] 0.1 g of caprolactam was dissolved in 100 ml of ultrapure water to prepare a 1000 ppm solution. This solution was further diluted to prepare standard solutions of 100, 50, 20, 10, 5, and 2 ppm, respectively, and a calibration curve was created. [HPLC conditions] Instrument: Hewlett-Packard HP1100 HPLC system, Column: Waters Pureisil 5μm C18 120Å 4.6mm×250mm (40℃), Detector: UV210nm, Injection volume: 10μl, Flow rate: 0.7ml / min, Elution: Methanol / water (volume ratio: 35 / 75) for 12 minutes, then switched to methanol / water (volume ratio: 100 / 0) over 3 minutes for 30 minutes, then switched back to methanol / water (volume ratio: 35 / 75) over 5 minutes for 20 minutes. [Calculation method] The amount of monomer extracted (mass %) was calculated by dividing the monomer concentration detected in the sample under the above conditions by the mass of the sample being measured.

[0113] (4) Cooling crystallization temperature Tc and full width at half maximum Using a PerkinElmer differential scanning calorimeter (input-compensated DSC8000), 10 mg of the obtained resin was weighed, heated from room temperature to 260°C at a heating rate of 10°C / min, held at 260°C for 10 minutes, and then cooled to 100°C at a cooling rate of 10°C / min to measure the cooling crystallization temperature. In the DSC curve with heat flow (mW) on the vertical axis and temperature on the horizontal axis, the temperature of the peak top during cooling was defined as Tc (°C), and the baseline was drawn from the high-temperature side, with the interval between two points at half the absolute value of Tc defined as the width at half maximum (°C).

[0114] (5) Content of terminal amino groups The films obtained in each example and comparative example were dissolved in a solvent (phenol / ethanol = 4 / 1 volume ratio), a fixed amount of 0.02N hydrochloric acid was added, and then the mixture was back-titrated with 0.02N sodium hydroxide solution.

[0115] (6) Content of terminal carboxyl groups The films obtained in each example and comparative example were dissolved in benzyl alcohol at 180°C, phenolphthalein indicator was added, and the mixture was titrated with a 0.02N potassium hydroxide ethanol solution.

[0116] (7) Evaluation of the number of dot defects in the 10% grayscale area of ​​semitone printing and evaluation of the expandability of the 40% grayscale area. [Printing process] The printing ink was prepared by mixing Rio Alpha R39 blue (manufactured by TOYOINK) with the diluent NKFS102 (TOYOINK), and adjusting the viscosity (at 23°C) so that it measured in 15 seconds using a Zahn cup #3. The printing roll film was prepared by slitting the film 500 mm to the left and right of the center in the TD direction. After applying the ink to the film using a gravure printing Helio engraved gradation change plate, it was dried at 50°C for 10 seconds and then wound up to produce the printing film. This tonal variation is helio-engraved with 175 lines (175 dots per inch width) in the MD direction in the order of 10%, 20%, 30%, 40%, and 100% tones. The depth of each tone is 2.5 μm, 5.0 μm, 7.5 μm, 10.0 μm, and 32.0 μm, respectively. The print length in the MD direction for each tone is 60 mm, and the print width in the TD direction is 0.8 m. Rio Alpha R39 Indigo has the following main components: 10% by mass of pigment, 15% by mass of synthetic resin, 2.5% by mass of silica, 30% by mass of ethyl acetate, 15% by mass of isopropyl alcohol, 10% by mass of propyl acetate, 10% by mass of propylene glycol monomethyl ether, and 5% by mass of n-propyl alcohol. The diluent NKFS102 has a main composition of 50% by mass of ethyl acetate, 35% by mass of propyl acetate, 10% by mass of isopropyl alcohol, and 5% by mass of n-propyl alcohol. [Number of dead pixels rating] Ten samples were taken from the 10% grayscale portion of the fabricated printed film. These samples were magnified 8 times using a stereomicroscope (ZEISS SteREO Discovery.V12) and measured over a total area of ​​1000 mm² (20 mm in the MD direction x 50 mm in the TD direction). 2 The number of missing dots (i.e., areas that could not be printed) within the specified range (a total of 47,500 dots) was counted. The same evaluation was performed at 10 sampled locations, and the value with the highest number of missing dots among all 10 locations is shown in Table 3. Figure 1 shows an overview of the measurement method. In the printed area with a 10% grayscale, the MD direction was evaluated at the remaining 20 mm portion excluding the top and bottom 20 mm, and the TD direction was evaluated at 10 points at 30 mm intervals, starting from 100 mm from the edge of the film, with the first point being at 50 mm. In other words, as shown in Figure 1, 10 points in the 20 mm × 50 mm measurement area a to j were evaluated. The number of missing dots should, practically speaking, be 100 or less out of a total of 47,500 dots, but preferably 80 or less, even more preferably 70 or less, and most preferably 60 or less. If the number of missing dots exceeds 100, even in the low-gradation areas, unevenness can be seen with the naked eye upon close inspection, individual differences in the design can be perceived, and it may be judged as a printing defect. [Scalability Assessment] The 40% grayscale portion of the prepared printed film was magnified 20 times using a stereomicroscope (ZEISS SteREO Discovery.V12), and the dot shape was observed. The dot diameters were measured at 10 arbitrary points and evaluated in three stages according to the following evaluation criteria. (Evaluation Criteria) ◎...No problems were observed with the halftone dot shape, and the ratio of the minimum to maximum halftone dot diameter was between 0.9 and 1. ○...No problems were observed with the halftone dot shape, and the ratio of the minimum to maximum halftone dot diameter was between 0.85 and less than 0.9. △...Slight distortion is observed in the halftone dot shape, and the ratio of the minimum to maximum halftone dot diameter is between 0.75 and 0.85. ×...The dot shape is distorted, there are inconsistencies in size, and the ratio of the minimum to maximum dot diameter is less than 0.75.

[0117] (8) Impact strength (J) The sample was cut from the central part of the obtained polyamide resin film, and from 50 cm to the left and right of the central part in the TD direction, resulting in sections measuring 10 cm wide x 150 cm long. Using a film impact tester manufactured by Toyo Seiki Seisakusho Co., Ltd., the sample was clamped and fixed in a jig with a 1 / 2-inch hemispherical head and a circular hole with a diameter of 50 cm, and the impact strength was measured 15 times for each section. The ratio of the minimum to maximum impact strength (minimum / maximum) is shown in Table 2. The ratio is preferably 0.5 to 1.0, more preferably 0.6 to 1.0, and even more preferably 0.7 to 1.0. If the ratio is less than 0.5, it is considered that there is a partial decrease in the impact resistance of the film, which is not practically desirable.

[0118] (10) Tensile elongation (%) Tensile elongation was measured using a Shimadzu DSS-500 autograph in accordance with Japanese Industrial Standard JIS K7127. A sample was obtained by cutting a 10 mm wide, 150 mm long section from the center of the polyamide resin film in the TD direction in the MD direction. Measurements were performed under conditions of a measurement length of 100 mm (distance between grips) and a tensile speed of 500 mm / min, and the elongation was calculated using the following formula. Tensile elongation (%) = Distance traveled by the grip at the time of fracture (mm) / Original distance between grips (100 mm) × 100

[0119] (11) Haze (%) A haze meter (NDH4000) manufactured by Nippon Denshoku Co., Ltd. was used to measure the central part of the film in the TD direction in accordance with the Japanese Industrial Standard JIS K7136.

[0120] (12) Wetting tension (mN / m) In accordance with Japanese Industrial Standard JIS K6768, the wetting tension was measured on the corona-treated surface of the film using a wet tensile strength test mixture No. 36.0~54.0 (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.). Measurements were taken at five locations in the TD direction, at 200 mm intervals from the center outwards to both ends. These measurements were then repeated every 1 m in the MD direction, for a total of 50 measurements. Table 3 shows the minimum and maximum wet tensile strength values ​​for these 50 locations. While a wet tensile strength of 44 mN / m or higher is generally practical, a strength of 46 mN / m or higher is particularly preferable.

[0121] (13) Bag tear resistance (bag drop test) [Lamination process] A urethane-based adhesive (DIC Corporation, DIC Dry LX-401A / SP-60) was applied to the surface of the film at a dry application rate of 3.0 g / m². 2 The adhesive was applied in this manner, and then heat-treated at 80°C. After heat treatment, an unstretched polyethylene film (TUX MCS, 50 μm, manufactured by Mitsui Chemicals Tohcello Co., Ltd.) was dry-laminated onto the adhesive surface at 80°C using a nip pressure of 490 kPa. Further aging as recommended by the adhesive was performed to obtain a laminated film. [Bag making sample creation] Two pieces of the prepared laminate film were cut to a size of 200mm x 300mm, the polyethylene films were joined together, and three sides were heat-sealed with a 10mm width to create a three-sided bag. The sealing conditions were 160°C for 1 second. 1000ml of water was filled into the prepared three-sided bag, the air inside the bag was released, the remaining side was heat-sealed with a 10mm width, then 10ml of air was injected using a syringe, and the bag was heat-sealed again to create a test sample. The sealing conditions were 160°C for 1 second. Adding a small amount of air increased the damage to the bag from the water, resulting in a more severe test condition compared to using only water. [Bag Drop Test] The prepared test sample was dropped from a height of 1.2 m above a horizontally placed 0.5 mm thick smooth stainless steel plate (SUS plate) with one film side of the sample hitting the SUS plate. This was followed by Test A, and then Test B, in which the sample was dropped with one short side hitting the SUS plate. These tests were repeated alternately until the sample burst, and the number of drops required for Test A or B to burst was measured. The test sample had two film surfaces and two short sides, and each sample was dropped so that either the same film surface or the same short side would hit the SUS plate. The test was conducted at 23°C and in a 50% RH atmosphere with a sample size of n=3, and the minimum number of drops until the bag bursts is shown in Table 3. Under these conditions, a practical number of drops until the bag bursts is required, preferably 50 or more, and more preferably 60 or more, with 70 or more being even more preferable.

[0122] [Table 3]

[0123] As is clear from these results, the biaxially oriented polyamide resin films of Examples 1 to 19 are polyamide resin films made using polyamide resin obtained by polymerizing recycled monomers, and therefore exhibit excellent printability in low-gradation areas, controlled variation in impact strength, and no problems with general physical properties such as film elongation, wettability, and haze, and also have excellent practical performance as shown in the drop bag test.

[0124] In Comparative Example 1, the relative viscosity of the raw materials used was low, resulting in reduced mechanical properties of the resulting film, particularly low impact strength. This led to cutting problems in the next process, preventing normal printing.

[0125] Comparative Examples 2, 4, and 5 did not contain polyamide resin polymerized from recycled monomers. They had a high amount of terminal amino groups or carboxyl groups derived from the remelted resin, which led to a faster crystallization rate of the film raw material. As a result, localized variations in the crystallization state of the surface occurred, which reduced the printability of low-gradation areas. In bag drop tests, this also led to a localized decrease in adhesion and increased bag tearing. Furthermore, a decrease in elongation and variations in impact strength were observed, which are thought to be due to impurities in the remelted resin.

[0126] Comparative Example 3, using the same raw materials as Comparative Example 2, underwent sequential stretching, resulting in an increase in the amount of monomer in the film. This led to a localized decrease in printability in low-gradation areas, and similarly, the results of the drop bag test also deteriorated. A decrease in elongation and variability in impact strength, which are thought to be due to impurities in the remelted resin, were also observed.

[0127] Comparative Example 6 is a film obtained using a polyamide resin composed solely of virgin monomers. While there were no problems with general physical properties or practical performance, the printability in low-gradation areas was inferior to that of the film using recycled monomers.

[0128] Comparative Example 7 used a polyamide resin consisting solely of virgin monomers. However, due to insufficient temperature control of the casting roll, variations occurred in the surface crystallinity of the unstretched film. As a result, variations in crystallinity also occurred on the surface of the stretched film, leading to a decrease in printability in low-gradation areas. Furthermore, the accuracy of the stretched film thickness exceeded 15% in some areas, which caused variations in impact strength and elongation.

Claims

1. A method for producing a polyamide 6 resin film, (1) A process of producing monomers from depolymerization raw materials (A), which are resin waste materials of polyamide resin. (2) A step of producing a polyamide 6 resin (B) having a cooling crystallization peak full width at half maximum of 10°C or more by polymerization using a raw material containing the monomer, (3) A step of refining the polyamide 6 resin (B) so that its relative viscosity (at 25°C) is in the range of 2.5 to 4.

5. (4) A process of preparing an unstretched film using a starting material containing refined polyamide 6 resin (B), and then biaxially stretching the unstretched film. A method for producing a polyamide 6 resin film, characterized by containing [the specified ingredient].

2. The manufacturing method according to claim 1, wherein the monomer comprises ε-caprolactam.

3. The manufacturing method according to claim 1, further comprising a step of adjusting the moisture content of the unstretched film to 2 to 10% by mass prior to stretching.

4. The manufacturing method according to claim 1, wherein the manufacturing method includes, as part of the starting material, a remelted resin obtained by melting a polyamide 6 resin (excluding the polyamide 6 resin (B)), and the content of the remelted resin is 1% by mass or more.

5. The manufacturing method according to claim 1, wherein the relative viscosity ηR of the polyamide 6 resin film is 2.5 to 4.

5.

6. The manufacturing method according to claim 1, wherein the depolymerizing raw material (A) is at least one of polyamide 6 resin and its oligomer.

Citation Information

Patent Citations

  • Method for casting nylon with polymonomer of waste nylon

    CN1058026A

  • Clothing product made of nylon and method for recycling the same

    JP1995310204A

  • Depolymerization of nylon 6 and apparatus therefor

    JP1995330718A

  • Recovery of epsilon-caprolactam