Method for producing positive electrode active material
Patent Information
- Application Number
- JP2022558369
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2020-11-17
- Filing Date
- 2021-10-13
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2041-10-13
AI Technical Summary
Lithium-ion secondary batteries face challenges in achieving high capacity, stability, and reliability due to the instability of positive electrode active materials at high potentials and temperatures, leading to reduced cycle life and safety concerns.
A method for producing a positive electrode active material by coating a first material, such as lithium cobalt oxide, with a second material like aluminum oxide or phosphate, which covers at least a portion of the particle surface, reducing direct contact with the electrolyte and enhancing stability and durability, and heat-treating in an oxygen-containing atmosphere to improve structural integrity and fire resistance.
The coated positive electrode active material exhibits improved charge-discharge cycle characteristics, increased stability at high voltages, and enhanced fire resistance, leading to more reliable and safe secondary batteries with increased durability and performance.
Abstract
Description
Method for producing positive electrode active material, positive electrode, secondary battery, electronic device, power storage system, and vehicle
[0001] BACKGROUND OF THE INVENTION 1. Field of the Invention One embodiment of the present invention relates to a method for manufacturing a positive electrode active material, a method for manufacturing a positive electrode, a method for manufacturing a secondary battery, or a portable information terminal, a power storage system, a vehicle, or the like including a secondary battery.
[0002] One embodiment of the present invention relates to an object, a method, or a manufacturing method. Alternatively, the present invention relates to a process, a machine, manufacture, or a composition of matter. Another embodiment of the present invention relates to a semiconductor device, a display device, a light-emitting device, a power storage device, a lighting device, an electronic device, or a manufacturing method thereof. Note that one embodiment of the present invention particularly relates to a method for manufacturing a positive electrode active material or a positive electrode active material. Alternatively, one embodiment of the present invention particularly relates to a method for manufacturing a positive electrode or a positive electrode. Alternatively, one embodiment of the present invention particularly relates to a method for manufacturing a secondary battery or a secondary battery.
[0003] In this specification, the term "semiconductor device" refers to any device that can function by utilizing semiconductor characteristics, and electro-optical devices, semiconductor circuits, and electronic devices are all included in the category of semiconductor devices.
[0004] In this specification, an electronic device refers to a device in general that has a positive electrode active material, a secondary battery, or a power storage device, and electro-optical devices that have a positive electrode active material, a positive electrode, a secondary battery, or a power storage device, and information terminal devices that have a power storage device are all electronic devices.
[0005] In this specification, the term "power storage device" refers to all elements and devices having a power storage function, including, for example, power storage devices such as lithium ion secondary batteries (also called secondary batteries), lithium ion capacitors, and electric double layer capacitors.
[0006] In recent years, various types of power storage devices have been actively developed, such as lithium-ion secondary batteries, lithium-ion capacitors, and air batteries. In particular, demand for high-power, high-energy-density lithium-ion secondary batteries has rapidly expanded in conjunction with the development of the semiconductor industry, and they are now indispensable in the modern information society as a rechargeable energy source, and are used in portable information terminals such as mobile phones, smartphones, and notebook computers, portable music players, digital cameras, medical devices, home energy storage systems, industrial energy storage systems, and next-generation clean energy vehicles such as hybrid vehicles (HVs), electric vehicles (EVs), and plug-in hybrid vehicles (PHVs).
[0007] Among these, composite oxides such as lithium cobalt oxide and lithium nickel-cobalt-manganese oxide, which have a layered rock salt structure, are widely used. These materials have useful properties as active materials for energy storage devices, such as high capacity and high discharge voltage. However, to achieve high capacity, the positive electrode must be exposed to a high potential relative to lithium during charging. Under such a high potential, large amounts of lithium are removed, which can reduce the stability of the crystal structure and lead to significant deterioration during charge-discharge cycles. Against this background, efforts have been made to improve the positive electrode active materials of secondary battery positive electrodes in order to develop high-capacity and highly stable secondary batteries (e.g., Patent Documents 1 to 3).
[0008] JP 2018-088400 A International Publication No. 2018 / 203168 Pamphlet JP 2020-140954 A
[0009] Toyoki Okumura et al, “Correlation of lithium ion distribution and X-ray absorption near-edge structure in O3-and O2-lithium cobalt oxides from first-principle calculation”, Journal of Materials Chemistry, 2012, 22, pp. 17340-17348 Motohashi, T. et al, “Electronic phase diagram of the layered cobalt oxide system LixCoO▲2▼(0.0≦x≦1.0)”, Physical Review B, 80 (16), 2009, 165114 Zhaohui Chen et al, “Staging Phase Transitions in LixCoO▲2▼”, Journal of The Electrochemical Society, 2002, 149(12) A1604-A1609W. E. Counts et al, Journal of the American Ceramic Society, 1953, 36 [1] pp. 12-17. Fig. 01471Belsky, A. et al. , “New developments in the Inorganic Crystal Structure Database (ICSD): accessibility in support of materials research and design”, Acta Crystal. , 2002, B58 pp. 364-369.
[0010] Although improvements to positive electrode active materials have been actively carried out in the above Patent Documents 1 to 3, there remains room for improvement in various aspects of lithium ion secondary batteries and positive electrode active materials used therein, such as charge / discharge capacity, cycle characteristics, reliability, safety, and cost.
[0011] In view of the above, an object of one embodiment of the present invention is to provide a method for manufacturing a positive electrode active material that is stable in a high potential state and / or a high temperature state. Another object is to provide a method for manufacturing a positive electrode active material whose crystal structure is not easily destroyed even after repeated charge and discharge. Another object is to provide a method for manufacturing a positive electrode active material that has excellent charge and discharge cycle characteristics. Another object is to provide a method for manufacturing a positive electrode active material that has large charge and discharge capacity. Another object is to provide a highly reliable or safe secondary battery.
[0012] Another object of one embodiment of the present invention is to provide a method for manufacturing a positive electrode that is stable in a high potential state and / or a high temperature state, a method for manufacturing a positive electrode that has excellent charge-discharge cycle characteristics, a method for manufacturing a positive electrode that has large charge-discharge capacity, or a secondary battery that is highly reliable or safe.
[0013] Another object of one embodiment of the present invention is to provide a novel substance, active material particles, an electrode, a secondary battery, a power storage device, or a manufacturing method thereof.Another object of one embodiment of the present invention is to provide a manufacturing method of a secondary battery or a secondary battery having one or more characteristics selected from high purity, high performance, and high reliability.
[0014] Note that the description of these problems does not preclude the existence of other problems. Note that one embodiment of the present invention does not necessarily solve all of these problems. Note that problems other than these can be extracted from the description of the specification, drawings, and claims.
[0015] A desirable form of the composite having a positive electrode active material is a structure in which at least a portion of the particle surface of a particulate first material functioning as a positive electrode active material is covered with a second material, and more desirably, a structure in which substantially the entire particle surface of the particulate first material is covered with the second material. Here, the state of substantially the entire coverage means a state in which the particulate first material and the electrolyte do not come into direct contact with each other.
[0016] When at least a portion, preferably substantially the entire surface, of the particles of the first material is covered with the second material, the area of direct contact between the first material and the electrolyte is reduced, thereby suppressing the desorption of transition metal elements and / or oxygen from the first material in a high-voltage charging state. This can suppress the capacity decrease due to repeated charging and discharging. Furthermore, when a material whose crystal structure is stable even in a high-voltage charging state is used as the second material, a secondary battery using the composite of one embodiment of the present invention can achieve effects such as improved stability at high temperatures and improved fire resistance.
[0017] Furthermore, by using a material that is stable under high-voltage charging as the first material, the durability and stability of the composite under high-voltage charging can be further improved, and the heat resistance and / or fire resistance of a secondary battery using the composite can be further improved.
[0018] As the first material, it is preferable to use, for example, lithium cobalt oxide and / or a metal oxide-coated composite oxide that is stable under high-voltage charging conditions. Examples of lithium cobalt oxide that is stable under high-voltage charging conditions include lithium cobalt oxide with added magnesium and fluorine, and lithium cobalt oxide with added magnesium, fluorine, aluminum, and nickel. Furthermore, it is preferable to use a metal oxide-coated composite oxide in which secondary particles of lithium nickel-cobalt-manganese oxide are coated with aluminum oxide. The nickel-cobalt-manganese lithium oxide can have an atomic ratio of nickel:cobalt:manganese=8:1:1 or nickel:cobalt:manganese=9:0.5:0.5.
[0019] Lithium cobalt oxide to which magnesium, fluorine, aluminum, and nickel are added is a particularly preferred material as the first material because it exhibits significantly excellent high-voltage charge / discharge cycle characteristics when subjected to the initial heating described below.
[0020] The second material covering at least a part of, and preferably almost the entire, particle surface of the first material is an oxide and LiM2PO 4 (M2 is one or more selected from Fe, Ni, Co, and Mn) can be used. Examples of oxides include aluminum oxide, zirconium oxide, hafnium oxide, and niobium oxide. Also, LiM2PO 4 (M2 is one or more selected from Fe, Ni, Co, and Mn) 4 , LiNiPO 4 , LiCoPO 4 , LiMnPO 4 , LiFe a Ni b P.O. 4 , LiFe a Co b P.O. 4 , LiFe a Mn b P.O. 4 , LiNi a Co b P.O. 4 , LiNi a Mn b P.O. 4 (a+b is 1 or less, 0<a<1, 0<b<1), LiFe c Ni d Co e P.O. 4 , LiFe c Ni d Mn e P.O. 4 , LiNi c Co d Mn e P.O. 4 (c+d+e is 1 or less, 0<c<1, 0<d<1, 0<e<1), LiFe f Ni g Co h Mn i P.O. 4 (f+g+h+i is 1 or less, 0<f<1, 0<g<1, 0<h<1, 0<i<1), etc.
[0021] The positive electrode of the present invention may have a structure in which at least a portion of the surface of the composite is covered with a graphene compound, preferably a structure in which 80% or more of the particle surfaces of the composite and / or aggregates containing the composite are covered with the graphene compound.
[0022] One aspect of the present invention is a semiconductor device comprising a first material and a second material covering at least a portion of a surface of the first material, the first material being LiMO 2 (M1 is one or more selected from Fe, Ni, Co, Mn, and Al), and the second material is LiM2PO 4 (M2 is one or more selected from Fe, Ni, Co, and Mn).
[0023] Another embodiment of the present invention includes a first material and a second material covering at least a part of a surface of the first material, the first material including lithium cobalt oxide containing magnesium, fluorine, aluminum, and nickel, and the second material including LiMPO 4 (M2 is one or more selected from Fe, Ni, Co, and Mn).
[0024] Another embodiment of the present invention provides a semiconductor device including a first material and a second material covering at least a part of a surface of the first material, the first material including lithium cobalt oxide containing magnesium, fluorine, aluminum, and nickel, the lithium cobalt oxide having a region in a surface layer portion where the concentration of magnesium, fluorine, or aluminum is maximum, and the second material including LiMPO 4 (M2 is one or more selected from Fe, Ni, Co, and Mn).
[0025] Another aspect of the present invention is a semiconductor device including a first material and a second material covering at least a part of a surface of the first material, the first material being LiMO 2 (M1 is one or more selected from Fe, Ni, Co, Mn, and Al), and the second material is aluminum oxide.
[0026] Another embodiment of the present invention is a positive electrode including a first material and a second material covering at least a part of a surface of the first material, in which the first material includes lithium cobalt oxide including magnesium, fluorine, aluminum, and nickel, and the second material includes aluminum oxide.
[0027] Another embodiment of the present invention is a positive electrode including a first material and a second material covering at least a part of a surface of the first material, wherein the first material includes lithium cobalt oxide containing magnesium, fluorine, aluminum, and nickel, and the lithium cobalt oxide has a region in a surface layer portion where the concentration of magnesium, fluorine, or aluminum is maximum, and the second material includes aluminum oxide.
[0028] Furthermore, one aspect of the present invention includes a first material and a second material, and the first material is LiMO 2 (M1 is one or more selected from Fe, Ni, Co, Mn, and Al), and the second material is LiM2PO 4 (M2 is one or more selected from Fe, Ni, Co, and Mn).
[0029] One embodiment of the present invention is a secondary battery including any one of the above positive electrodes.
[0030] One embodiment of the present invention is a vehicle including the above secondary battery.
[0031] One embodiment of the present invention is a power storage system including the above secondary battery.
[0032] One embodiment of the present invention is an electronic device including the above secondary battery.
[0033] Another aspect of the present invention is a method for manufacturing a positive electrode active material including a first material and a second material, the method including: a first step of covering at least a portion of a surface of the first material with the second material to form a composite; and a second step of heating the composite, in which the first material includes lithium cobalt oxide including magnesium, fluorine, aluminum, and nickel, and the second material is LiMPO 4(M2 is one or more selected from Fe, Ni, Co, and Mn), and the heating is performed in an oxygen-containing atmosphere.
[0034] Another embodiment of the present invention is a method for manufacturing a positive electrode active material having a first material and a second material, the method including: a first step of covering at least a portion of a surface of the first material with the second material to form a composite; and a second step of heating the composite, in which the first material includes lithium cobalt oxide having magnesium, fluorine, aluminum, and nickel, and the second material includes aluminum oxide, and the heating is performed in an atmosphere containing oxygen.
[0035] In one aspect of the present invention, in any one of the above, the heating is preferably performed at a temperature of 450° C. or higher and 800° C. or lower.
[0036] According to one embodiment of the present invention, a method for manufacturing a positive electrode active material that is stable at a high potential and / or a high temperature can be provided. Alternatively, a method for manufacturing a positive electrode active material whose crystal structure is not easily destroyed even after repeated charge and discharge can be provided. Alternatively, a method for manufacturing a positive electrode active material that has excellent charge and discharge cycle characteristics can be provided. Alternatively, a method for manufacturing a positive electrode active material that has a large charge and discharge capacity can be provided. Alternatively, a highly reliable or safe secondary battery can be provided.
[0037] According to one embodiment of the present invention, a novel substance, active material particles, a secondary battery, a power storage device, or a manufacturing method thereof can be provided. According to another embodiment of the present invention, a manufacturing method of a secondary battery or a secondary battery having one or more characteristics selected from high purity, high performance, and high reliability can be provided.
[0038] Note that the description of these effects does not preclude the existence of other effects. Note that one embodiment of the present invention does not necessarily have all of these effects. Note that effects other than these will become apparent from the description in the specification, drawings, claims, etc., and it is possible to extract other effects from the description in the specification, drawings, claims, etc.
[0039] FIGS. 1A to 1C are diagrams illustrating an example of a method for manufacturing a positive electrode active material of one embodiment of the present invention. FIGS. 2A and 2B are diagrams illustrating calculations of an example of a positive electrode active material of one embodiment of the present invention. FIGS. 3A to 3C are diagrams illustrating calculations of an example of a positive electrode active material of one embodiment of the present invention. FIG. 4 is a diagram illustrating calculations of an example of a positive electrode active material of one embodiment of the present invention. FIGS. 5A and 5B are diagrams illustrating calculations of an example of a positive electrode active material of one embodiment of the present invention. FIGS. 6A and 6B are diagrams illustrating an example of a method for manufacturing a positive electrode of one embodiment of the present invention. FIGS. 7A and 7B are diagrams illustrating an example of a method for manufacturing a positive electrode of one embodiment of the present invention. FIG. 8 is a diagram illustrating an example of a method for manufacturing a positive electrode of one embodiment of the present invention. FIG. 9 is a diagram illustrating an example of a method for manufacturing a positive electrode of one embodiment of the present invention. FIGS. 10A and 10B are diagrams illustrating an example of a method for manufacturing a positive electrode active material of one embodiment of the present invention. FIGS. 11A to 11C are diagrams illustrating an example of a method for manufacturing a positive electrode active material of one embodiment of the present invention. FIG. 12 illustrates an example of a method for manufacturing a cathode active material of one embodiment of the present invention. FIGS. 13A to 13C illustrate an example of a method for manufacturing a cathode active material of one embodiment of the present invention. FIGS. 14A to 14C illustrate a method for manufacturing a cathode active material. FIG. 15 illustrates a method for manufacturing a cathode active material. FIGS. 16A to 16C illustrate a method for manufacturing a cathode active material. FIG. 17A is a top view of a cathode active material of one embodiment of the present invention, and FIG. 17B is a cross-sectional view of the cathode active material of one embodiment of the present invention. FIG. 18 illustrates the Li occupancy and crystal structure of a cathode active material of one embodiment of the present invention. FIG. 19 illustrates an XRD pattern calculated from the crystal structure. FIG. 20 illustrates the Li occupancy and crystal structure of a comparative cathode active material. FIG. 21 illustrates an XRD pattern calculated from the crystal structure. FIGS. 22A to 22C illustrate lattice constants calculated from XRD. 23A to 23C show lattice constants calculated from XRD. FIG. 24 is a graph of charge capacity and voltage. FIG. 25A is a graph of dQ / dV for a secondary battery of one embodiment of the present invention. FIG. 25B is a graph of dQ / dV for a secondary battery of one embodiment of the present invention. FIG. 25C is a graph of dQ / dV for a secondary battery of a comparative example. FIG. 26 is a cross-sectional schematic diagram of a positive electrode active material. FIGS. 27A and 27B are SEM images of a positive electrode.FIG. 28A is a front view showing three-dimensional information, FIG. 28B is an enlarged view of a portion thereof, FIG. 28C is a cross-sectional view thereof, FIG. 28D is a side view showing three-dimensional information, FIG. 28E is an enlarged view of a portion thereof, and FIG. 28F is a cross-sectional view thereof. FIGS. 29A to 29C are SEM images of the positive electrode. FIGS. 30A to 30C are SEM images of the positive electrode. FIGS. 31A and 31B are STEM images of the positive electrode. FIGS. 32A to 32C are EDX analysis results of the positive electrode. FIGS. 33A and 33B are cross-sectional TEM images of the positive electrode active material layer. FIGS. 34A to 34C are microelectron diffraction images of the positive electrode active material layer. FIGS. 35A to 35C are diagrams illustrating an example of a crystal structure. FIG. 36A is a cross-sectional STEM image of a particle after pressing, and FIGS. 36B and 36C are cross-sectional schematic views. FIG. 37 illustrates an example of a manufacturing method for a positive electrode active material of one embodiment of the present invention. FIG. 38 is a diagram illustrating an example of a method for manufacturing a cathode active material of one embodiment of the present invention. FIGS. 39A to 39E are diagrams illustrating an example of a method for manufacturing a cathode active material of one embodiment of the present invention. FIG. 40 is a diagram illustrating an example of a method for manufacturing a cathode active material of one embodiment of the present invention. FIG. 41 is a diagram illustrating an example of a method for manufacturing a cathode active material of one embodiment of the present invention. FIG. 42 is a diagram illustrating an example of a method for manufacturing a cathode active material of one embodiment of the present invention. FIG. 43 is a diagram illustrating an example of a method for manufacturing a cathode active material of one embodiment of the present invention. FIG. 44 is a diagram illustrating an example of a method for manufacturing a cathode active material of one embodiment of the present invention. FIG. 45 is a diagram illustrating an example of a method for manufacturing a cathode active material of one embodiment of the present invention. FIG. 46 is a diagram illustrating an example of a method for manufacturing a cathode active material of one embodiment of the present invention. FIG. 47 is a diagram illustrating an example of a method for manufacturing a cathode active material of one embodiment of the present invention. FIGS. 48A and 48B are cross-sectional views of a cathode active material. FIGS. 49A to 49C are diagrams illustrating concentration distributions in a cathode active material. FIG. 50 illustrates an example of a method for manufacturing a positive electrode active material of one embodiment of the present invention. FIG. 51 illustrates an example of a method for manufacturing a positive electrode active material of one embodiment of the present invention. FIG. 52 illustrates an example of a positive electrode of one embodiment of the present invention. FIG. 53A is an exploded perspective view of a coin-type secondary battery, FIG. 53B is a perspective view of the coin-type secondary battery, and FIG. 53C is a cross-sectional perspective view thereof. FIG. 54A illustrates an example of a cylindrical secondary battery.FIG. 54B shows an example of a cylindrical secondary battery. FIG. 54C shows an example of multiple cylindrical secondary batteries. FIG. 54D shows an example of a power storage system including multiple cylindrical secondary batteries. FIGS. 55A and 55B are diagrams illustrating an example of a secondary battery, and FIG. 55C is a diagram illustrating the internal state of the secondary battery. FIGS. 56A to 56C are diagrams illustrating an example of a secondary battery. FIGS. 57A and 57B are diagrams illustrating the appearance of a secondary battery. FIGS. 58A to 58C are diagrams illustrating a manufacturing method of a secondary battery. FIGS. 59A to 59C are diagrams illustrating a configuration example of a battery pack. FIGS. 60A and 60B are diagrams illustrating an example of a secondary battery. FIGS. 61A to 61C are diagrams illustrating an example of a secondary battery. FIGS. 62A and 62B are diagrams illustrating an example of a secondary battery. FIG. 63A is a perspective view of a battery pack illustrating one embodiment of the present invention, FIG. 63B is a block diagram of the battery pack, and FIG. 63C is a block diagram of a vehicle having a motor. 64A to 64D are diagrams illustrating an example of a transportation vehicle. FIGS. 65A and 65B are diagrams illustrating a power storage device according to one embodiment of the present invention. FIG. 66A is a diagram illustrating an electric bicycle, FIG. 66B is a diagram illustrating a secondary battery for the electric bicycle, and FIG. 66C is a diagram illustrating an electric motorcycle. FIGS. 67A to 67D are diagrams illustrating an example of an electronic device. FIG. 68A shows an example of a wearable device, FIG. 68B is a perspective view of a wristwatch-type device, and FIG. 68C is a diagram illustrating a side view of the wristwatch-type device. FIG. 68D is a diagram illustrating an example of a wireless earphone. FIGS. 69A to 69C are SEM images of the surface of a positive electrode active material. FIGS. 70A and 70B are graphs illustrating cycle characteristics.
[0040] Hereinafter, embodiments of the present invention will be described in detail with reference to the drawings. However, the present invention is not limited to the following description, and it will be readily understood by those skilled in the art that various modifications can be made to the embodiments and details. Furthermore, the present invention should not be interpreted as being limited to the description of the embodiments shown below.
[0041] A secondary battery has, for example, a positive electrode and a negative electrode. A material constituting the positive electrode is a positive electrode active material. The positive electrode active material is, for example, a substance that undergoes a reaction that contributes to the charge / discharge capacity. Note that the positive electrode active material may contain a substance that does not contribute to the charge / discharge capacity.
[0042] In this specification and the like, the positive electrode active material of one embodiment of the present invention may be referred to as a positive electrode material, a positive electrode material for a secondary battery, a composite oxide, or the like. Furthermore, in this specification and the like, the positive electrode active material of one embodiment of the present invention preferably includes a compound. Furthermore, in this specification and the like, the positive electrode active material of one embodiment of the present invention preferably includes a composition. Furthermore, in this specification and the like, the positive electrode active material of one embodiment of the present invention preferably includes a composite including the positive electrode active material.
[0043] Furthermore, in this specification and the like, the term "particle" is not limited to referring only to spherical shapes (having a circular cross-sectional shape), and examples of the cross-sectional shape of individual particles include ellipsoids, rectangles, trapezoids, cones, squares with rounded corners, and asymmetric shapes, and further, individual particles may have an irregular shape.
[0044] The particle size can be measured, for example, by laser diffraction particle size distribution measurement, and the D50 value can be used for comparison. Here, D50 refers to the particle size at which the cumulative amount in the cumulative particle amount curve of the particle size distribution measurement results accounts for 50%, i.e., the median. The measurement of particle size is not limited to laser diffraction particle size distribution measurement; when the particle size is below the lower measurement limit of laser diffraction particle size distribution measurement, the major axis of the particle cross section may be measured by analysis using a scanning electron microscope (SEM) or a transmission electron microscope (TEM).
[0045] Furthermore, in this specification and the like, Miller indices are used to represent crystal planes and directions. Individual planes indicating crystal planes are represented in parentheses. In crystallography, crystal planes, directions, and space groups are represented by adding a superscript bar to the numbers, but in this specification and the like, due to restrictions on notation in applications, numbers may be represented by adding a - (minus sign) before them instead of adding a bar above them.
[0046] In this specification, the layered rock-salt type crystal structure of a composite oxide containing lithium and a transition metal refers to a crystal structure having a rock-salt type ion arrangement in which cations and anions are alternately arranged, and in which the transition metal and lithium are regularly arranged to form a two-dimensional plane, allowing two-dimensional diffusion of lithium. Defects such as cation or anion deficiencies may also be present. Strictly speaking, the layered rock-salt type crystal structure may have a distorted rock-salt type crystal lattice.
[0047] In this specification and the like, the rock salt type crystal structure refers to a structure in which cations and anions are arranged alternately. Note that the crystal structure may have a deficiency of cations or anions in part.
[0048] In this specification, the theoretical capacity of a positive electrode active material refers to the amount of electricity when all of the intercalable and deintercalable lithium contained in the positive electrode active material is deintercalated. For example, LiFePO 4 The theoretical capacity of LiCoO is 170 mAh / g. 2 The theoretical capacity of LiNiO is 274 mAh / g. 2 The theoretical capacity of LiMn is 274mAh / g. 2 O 4 The theoretical capacity of the battery is 148 mAh / g.
[0049] In this specification and the like, the amount of lithium remaining in the positive electrode active material that can be inserted or removed is determined by x in the composition formula, for example, Li x CoO 2 x in, or Li x MO 2 In this specification, Li x CoO 2 Li as appropriate x MO 2 In the case of a positive electrode active material in a secondary battery, x can be expressed as x = (theoretical capacity - charging capacity) / theoretical capacity. For example, LiCoO 2 When a secondary battery using as a positive electrode active material is charged at 219.2 mAh / g, Li 0.2 CoO 2 Or we can say x = 0.2. x CoO 2The small value of x in the formula means, for example, 0.1<x≦0.24.
[0050] When properly synthesized lithium cobalt oxide is used in the positive electrode, the stoichiometric ratio is approximately satisfied. 2 and the occupancy rate of Li on the lithium site is x = 1. In addition, the secondary battery after discharge is also LiCoO 2 In this case, the discharge is completed when the voltage reaches 2.5 V (vs. Li / Li) at a discharge current of 100 mA / g. + ) refers to the following state:
[0051] Although the present specification and the like may show examples of secondary batteries using a positive electrode and a positive electrode active material of one embodiment of the present invention, in which lithium metal is used for the negative electrode, the secondary battery of one embodiment of the present invention is not limited thereto. Other materials, such as graphite and lithium titanate, may also be used for the negative electrode. The properties of the positive electrode and positive electrode active material of one embodiment of the present invention, such as their resistance to crystal structure collapse even after repeated charge and discharge and their excellent cycle characteristics, are not affected by the material of the negative electrode. Although examples of secondary batteries of one embodiment of the present invention in which the secondary battery is charged and discharged at a relatively high voltage, such as a charge voltage of 4.6 V, using a lithium counter electrode, may also be shown. Charge and discharge at a lower voltage is expected to result in even better cycle characteristics than those shown in the present specification and the like.
[0052] In this specification, the term "kiln" refers to a device for heating an object to be treated. For example, the term "kiln" may be replaced with a furnace, a kiln, a heating device, or the like.
[0053] Embodiment 1 In this embodiment, a composite including a positive electrode active material of one embodiment of the present invention, a method for manufacturing the composite, and a method for manufacturing a positive electrode will be described.
[0054] 1A to 1C are diagrams illustrating a method for fabricating a composite having a positive electrode active material. Also, FIGS. 2A to 5B are diagrams relating to calculations of a composite having a positive electrode active material. Also, FIGS. 6A to 9 are diagrams illustrating a method for fabricating a positive electrode.
[0055] The positive electrode includes a positive electrode active material layer and a positive electrode current collector. The positive electrode active material layer includes a composite including a first material that functions as a positive electrode active material and a second material that covers at least a portion of the first material, and may further include a conductive agent and a binder. Note that the composite including the positive electrode active material may also be simply referred to as the positive electrode active material.
[0056] The composite having the positive electrode active material can be obtained by a composite treatment described below using at least a first material and a second material. Examples of the composite treatment include composite treatments using mechanical energy, such as mechanochemical, mechanofusion, and ball milling; composite treatments using liquid-phase reactions, such as coprecipitation, hydrothermal, and sol-gel; and composite treatments using gas-phase reactions, such as barrel sputtering, ALD (Atomic Layer Deposition), vapor deposition, and CVD (Chemical Vapor Deposition). It is preferable to perform a heat treatment after the composite treatment. In this specification, the composite treatment is also referred to as a surface coating treatment or a coating treatment.
[0057] When a heat treatment is performed after the composite formation process, the second material covering at least a portion of the first material is sintered or melted and spread, which is expected to reduce the number of points of direct contact between the first material and the electrolyte. On the other hand, if the temperature of the heat treatment after the composite formation process is too high, the elements of the second material may diffuse more than necessary into the first material, which may reduce the charge / discharge capacity of the first material and reduce the effectiveness of the second material as a coating layer. Therefore, when a heat treatment is performed after the composite formation process, it is necessary to appropriately set the heating temperature, heating time, and heating atmosphere.
[0058] In the composite manufacturing method 1, a first material 100x and a second material 100y are combined by a mechanical energy process, but the present invention is not limited to the above description.
[0059] [Method 1 for Preparing Composite] An example of a method for preparing a composite including a positive electrode active material according to one embodiment of the present invention will be described with reference to FIGS. 1A to 1C. FIG.
[0060] In step S101 of FIG. 1A, a first material 100x is prepared, and in step S102, a second material 100y is prepared.
[0061] The first material 100x is LiMO prepared by the method shown in the third embodiment described later. 2 (M1 is one or more selected from Fe, Ni, Co, Mn, and Al), to which an additive element X has been added, can be used. For example, lithium cobalt oxide to which magnesium and fluorine have been added, or lithium cobalt oxide to which magnesium, fluorine, aluminum, and nickel have been added, can be used. In particular, lithium cobalt oxide to which magnesium, fluorine, aluminum, and nickel have been added is preferably one that has undergone the initial heating process described in embodiment 3. Another example of the first material 100x is lithium nickel-cobalt-manganese oxide. Here, the transition metal ratio of the lithium nickel-cobalt-manganese oxide is preferably a high nickel ratio. For example, a material having an atomic ratio of nickel:cobalt:manganese=8:1:1 or nickel:cobalt:manganese=9:0.5:0.5 is preferred. Furthermore, a metal oxide-coated composite oxide can be used, in which secondary particles of lithium nickel-cobalt-manganese oxide are coated with aluminum oxide. Here, the coating layer (aluminum oxide) of the metal oxide-coated composite oxide is preferably thin, for example, from 1 nm to 200 nm, more preferably from 1 nm to 100 nm. Furthermore, the nickel-cobalt-manganese lithium oxide preferably contains calcium-added nickel-cobalt-manganese lithium.
[0062] As the second material 100y, LiM2PO 4 (M2 is one or more selected from Fe, Ni, Co, and Mn). Alternatively, an oxide can be used as the second material 100y. Examples of oxides that can be used include aluminum oxide, zirconium oxide, hafnium oxide, and niobium oxide. LiM2PO4 Materials such as those mentioned above as LiFePO 4 , LiMnPO 4 , LiFe a Mn b P.O. 4 (a+b is 1 or less, 0<a<1, 0<b<1), LiFe a Ni b P.O. 4 (a+b is 1 or less, 0<a<1, 0<b<1) can be used. Furthermore, the particle surfaces of the second material 100y may have a carbon coating layer.
[0063] When a material that functions as a positive electrode active material is used as the second material 100y, it is possible to select a combination of the first material 100x and the second material 100y that is unlikely to cause a step in the charge / discharge curve, depending on the characteristics required of the secondary battery, or a combination that causes a step in the charge / discharge curve at a desired charging rate.
[0064] Next, in step S103, the first material 100x and the second material 100y are combined. When the combining process is performed using mechanical energy, the combining process can be performed by a mechanochemical method. Alternatively, the combining process can be performed by a mechanofusion method.
[0065] Furthermore, when a ball mill is used in step S103, it is preferable to use zirconia balls as media. If the ball mill process is intended for mixing, a dry process is preferable. When the ball mill process is performed in a wet process, acetone can be used. When performing a wet ball mill process, it is recommended to use dehydrated acetone with a moisture content of 100 ppm or less, preferably 10 ppm or less.
[0066] The composite treatment in step S103 makes it possible to create a state in which at least a portion, and preferably almost the entire surface of the particles of the first material 100x in particulate form is covered with the second material 100y.
[0067] Through the above steps, the composite 100z having the positive electrode active material of one embodiment of the present invention shown in FIG. 1A can be produced (step S104). Here, the composite 100z having the positive electrode active material obtained here may sometimes be simply referred to as the positive electrode active material.
[0068] In the production method shown in FIG. 1B, up to step S103 is the same as the production method shown in FIG. 1A. After step S103, a heat treatment is performed as step S104. The heating in step S104 is preferably carried out under the conditions of 400°C or higher and 950°C or lower, more preferably 450°C or higher and 800°C or lower, for 1 hour or longer and 60 hours or shorter, more preferably 2 hours or longer and 20 hours or shorter, in an atmosphere containing oxygen.
[0069] Through the above steps, the composite 100z having the positive electrode active material of one embodiment of the present invention shown in FIG. 1B can be produced (step S105). Here, the composite 100z having the positive electrode active material obtained here may sometimes be simply referred to as the positive electrode active material.
[0070] In the composite formation process, in order to obtain a good coating state, the ratio (particle diameter of the second material 100y / particle diameter of the first material 100x) of the particle diameter of the second material 100y to the particle diameter of the first material 100x is preferably 1 / 100 or more and 1 / 50 or less, and more preferably 1 / 200 or more and 1 / 100 or less. As for adjusting the particle diameter of the second material 100y, a micronization process may be performed by the method shown in FIG. 1C.
[0071] [Calculation 1 Regarding Composite] As an example calculation of a composite having a positive electrode active material, LiCoO 2 and LiFePO 4 and the structure in which they are combined, and LiCoO 2 and LiFe 0.5 Mn 0.5 PO 4 Or LiFe 0.5 Ni 0.5 PO 4 The structures in which they are combined were optimized and evaluated using the density functional method (DFT: Density Functional Theory). The main calculation conditions are shown in Table 1, and the initial states of the models used in the calculation are shown in FIGS. 2A and 2B.
[0072]
[0073] As the initial state of the model used for the calculation, LiCoO 2 and LiFePO 4 The structure of LiCoO is shown in FIG. 2 and LiFe 0.5 Mn 0.5 P.O. 4 or LiFe 0.5 Ni 0.5 P.O. 4 The potential difference before and after the extraction of Li (corresponding to the potential difference during charging) was calculated for these structural models. The results of the calculations are shown in graphs of theoretical capacity versus charging voltage in Figures 3A, 3B, and 3C.
[0074] As a result of calculation shown in FIGS. 3A, 3B, and 3C, the charging voltage is 4 <LiMnPO 4 <LiNiPO 4 It was confirmed that the increase in the order of LiFePO 4 Rather than LiFePO 4 When part of the Fe in LiFePO is replaced with Mn, the charging voltage is higher. 4 It was confirmed that when a part of the Fe in the above-mentioned battery was replaced with Ni, the charging voltage tended to be even higher.
[0075] [Calculation 2 for Composite] In a composite in which the particle surfaces of a first material 100x are covered with a second material 100y, the lattice distortion at the interface between the first material 100x and the second material 100y was verified by first-principles calculation.
[0076] Here, the first material 100x is LiNi 8/10 Co 1/10 Mn 1/10 O 2 (Ni:Co:Mn=8:1:1), the second material 100y is LiFePO 4 The calculation was carried out for the structure (hereinafter referred to as NCM-LFP junction). 8/10 Co 1/10 Mn 1/10 O 2LiFePO 4 The particles have a structure in which the (001) planes of the particles are joined together. 8/10 Co 1/10 Mn 1/10 O 2 : LiFePO 4 The ratio was set to 9:1.
[0077] Also, LiNi 8/10 Co 1/10 Mn 1/10 O 2 Particles only (hereinafter referred to as NCM only) and LiFePO 4 The particles alone (hereinafter referred to as LFP alone) were also examined.
[0078] Also, LiNi 8/10 Co 1/10 Mn 1/10 O 2 Particles and LiFePO 4 The case where the particles were mixed without bonding (hereinafter referred to as NCM-LFP mixture) was also investigated. 8/10 Co 1/10 Mn 1/10 O 2 : LiFePO 4 The ratio was set to 9:1.
[0079] First, optimization calculations were performed using density functional theory (DFT). The main calculation conditions are shown in Table 2. The numbers of atoms used in the calculations were 116 Li, 82 Ni, 11 Co, 11 Mn, 12 Fe, 12 P, and 256 O for the NCM-LFP junction. For the NCM-only junction, the numbers were 60 Li, 48 Ni, 6 Co, 6 Mn, and 120 O. For the LFP-only junction, the numbers were 32 Li, 32 Fe, 32 P, and 128 O.
[0080]
[0081] The state of the bonding interface after the optimization calculation is shown in FIG. 4. As shown as region 991 in FIG. 4, in the vicinity of the bonding interface, LiFePO 4 By joining with LiNi 8/10 Co 1/10Mn 1/10 O 2 The structure was observed to be distorted.
[0082] Next, the potential difference (corresponding to the potential difference during charging) before and after the extraction of lithium atoms was calculated for the optimized structure. For the NCM-LFP mixture, the potential difference for NCM alone was multiplied by the potential difference for LFP alone.
[0083] The calculated relationship between theoretical capacity and charging voltage is shown in Fig. 5A. Fig. 5B shows an enlarged view of a portion of the graph in Fig. 5A.
[0084] LiNi 8/10 Co 1/10 Mn 1/10 O 2 LiFePO on the surface of (Ni:Co:Mn=8:1:1) 4 In the structure where LiNi is bonded, the change in charging voltage with respect to capacitance is linear. This is because, as mentioned in Figure 4, 8/10 Co 1/10 Mn 1/10 O 2 This is thought to be because the structure of the alloy is distorted, weakening the interaction between the nickel and cobalt atoms.
[0085] [Positive Electrode Active Material] As the first material 100x, LiMO having a layered rock salt crystal structure 2 (M1 is one or more selected from Fe, Ni, Co, Mn, and Al) can be used as the first material 100x. 2A composite oxide represented by the formula (I) to which an additive element X is added can be used. The additive element X contained in the first material 100x is preferably one or more selected from nickel, cobalt, magnesium, calcium, chlorine, fluorine, aluminum, manganese, titanium, zirconium, yttrium, vanadium, iron, chromium, niobium, lanthanum, hafnium, zinc, silicon, sulfur, phosphorus, boron, and arsenic. These elements may further stabilize the crystal structure of the first material 100x. That is, the first material 100x can include lithium cobalt oxide doped with magnesium and fluorine, lithium cobalt oxide doped with magnesium, fluorine, aluminum, and nickel, lithium cobalt oxide doped with magnesium, fluorine, and titanium, lithium nickel-cobalt oxide doped with magnesium and fluorine, lithium cobalt-aluminate doped with magnesium and fluorine, lithium nickel-cobalt-aluminate, lithium nickel-cobalt-aluminate, lithium nickel-cobalt-aluminate doped with magnesium and fluorine, and lithium nickel-cobalt-manganate doped with magnesium and fluorine. The transition metal ratio of the lithium nickel-cobalt-manganate is preferably high, and materials with atomic ratios of, for example, nickel:cobalt:manganese = 8:1:1 or nickel:cobalt:manganese = 9:0.5:0.5 are preferred. Furthermore, the lithium nickel-cobalt-manganate preferably includes lithium nickel-cobalt-manganate doped with calcium.
[0086] Also, as the first material 100x, LiMO 2 Secondary particles of a composite oxide represented by the formula (where M1 is one or more selected from Fe, Ni, Co, Mn, and Al) coated with a metal oxide may also be used. The metal oxide may be an oxide of one or more metals selected from Al, Ti, Nb, Zr, La, and Li. For example, LiMO 2A metal oxide-coated complex oxide in which secondary particles of a complex oxide represented by the formula (M1) (where M1 is one or more selected from Fe, Ni, Co, Mn, and Al) are coated with aluminum oxide can be used as the first material 100x. For example, a metal oxide-coated complex oxide in which secondary particles of lithium nickel-cobalt-manganese oxide having an atomic ratio of nickel:cobalt:manganese = 8:1:1 or nickel:cobalt:manganese = 9:0.5:0.5 are coated with aluminum oxide can be used. Here, the coating layer is preferably thin, for example, 1 nm or more to 200 nm or less, more preferably 1 nm or more to 100 nm or less. Furthermore, the lithium nickel-cobalt-manganese oxide preferably includes calcium-added lithium nickel-cobalt-manganese oxide.
[0087] The first material 100x can be formed by the formation methods described in Embodiments 3 and 4 below.
[0088] The second material 100y is an oxide and LiM2PO4 having an olivine-type crystal structure. 4 (M2 is one or more selected from Fe, Ni, Co, and Mn) can be used (also called a composite oxide having an olivine-type crystal structure (having one or more selected from Fe, Ni, Co, and Mn)). Examples of oxides include aluminum oxide, zirconium oxide, hafnium oxide, and niobium oxide. Also, LiM2PO 4 As an example, LiFePO 4 , LiNiPO 4 , LiCoPO 4 , LiMnPO 4 , LiFe a Ni b P.O. 4 , LiFe a Co b P.O. 4 , LiFe a Mn b P.O. 4 , LiNi a Co b P.O. 4 , LiNi a Mn b P.O. 4(a+b is 1 or less, 0<a<1, 0<b<1), LiFe c Ni d Co e P.O. 4 , LiFe c Ni d Mn e P.O. 4 , LiNi c Co d Mn e P.O. 4 (c+d+e is 1 or less, 0<c<1, 0<d<1, 0<e<1), LiFe f Ni g Co h Mn i P.O. 4 (f+g+h+i is 1 or less, 0<f<1, 0<g<1, 0<h<1, 0<i<1), etc. Also, the particle surface of the second material 100y may have a carbon coating layer. LiM2PO having an olivine type crystal structure 4 (M2 is one or more selected from Fe, Ni, Co, and Mn) can be formed by the method described in Embodiment 5 below.
[0089] [Composite] In this embodiment, an example of a method for producing a composite in which at least a portion of the particle surface of a particulate first material 100x that functions as a positive electrode active material is covered with a second material 100y is shown in the above-mentioned composite production method 1. A desirable form of a composite having a positive electrode active material is a structure in which at least a portion of the particle surface of the particulate first material 100x is covered with the second material 100y, and more preferably a structure in which substantially the entire particle surface of the particulate first material 100x is covered with the second material 100y. Here, the state in which substantially the entire particle surface is covered means that the particulate first material 100x and the electrolyte do not come into direct contact with each other.
[0090] When at least a portion, preferably substantially the entire surface, of a particulate first material 100x that functions as a positive electrode active material is covered with the second material 100y, the area in direct contact with the electrolyte of the first material 100x is reduced. Therefore, desorption of transition metal elements and / or oxygen from the first material 100x during high-voltage charging can be suppressed, thereby suppressing capacity loss due to repeated charge and discharge. Furthermore, by covering the first material 100x with the second material 100y, whose crystal structure is stable even during high-voltage charging, a secondary battery using a composite having the positive electrode active material of one embodiment of the present invention can achieve effects such as improved stability at high temperatures and improved fire resistance.
[0091] In particular, by using a material having excellent stability under high-voltage charging as the first material 100x, the durability and stability of the composite under high-voltage charging can be further improved, and the heat resistance and / or fire resistance of a secondary battery using the composite can be further improved.
[0092] As a material having excellent stability under high-voltage charging conditions, it is preferable to use lithium cobalt oxide to which magnesium and fluorine are added, or lithium cobalt oxide to which magnesium, fluorine, aluminum, and nickel are added. Furthermore, as a material having excellent stability under high-voltage charging conditions, it is preferable to use a metal oxide-coated composite oxide in which secondary particles of nickel-cobalt-manganese lithium oxide are coated with aluminum oxide. The atomic ratio of nickel-cobalt-manganese lithium oxide can be, for example, nickel:cobalt:manganese = 8:1:1, or nickel:cobalt:manganese = 9:0.5:0.5.
[0093] Lithium cobalt oxide doped with magnesium, fluorine, aluminum, and nickel exhibits significantly superior high-voltage charge / discharge cycle characteristics when subjected to the initial heating described below, and is therefore a particularly preferred material for the first material 100x.
[0094] The second material, which covers at least a part of, and preferably almost the entire, particle surface of the particulate first material 100x that functions as a positive electrode active material, is an oxide and LiM2PO 4(M2 is one or more selected from Fe, Ni, Co, and Mn). Examples of oxides include aluminum oxide, zirconium oxide, hafnium oxide, and niobium oxide. Also, LiM2PO 4 (M2 is one or more selected from Fe, Ni, Co, and Mn) 4 , LiNiPO 4 , LiCoPO 4 , LiMnPO 4 , LiFe a Ni b P.O. 4 , LiFe a Co b P.O. 4 , LiFe a Mn b P.O. 4 , LiNi a Co b P.O. 4 , LiNi a Mn b P.O. 4 (a+b is 1 or less, 0<a<1, 0<b<1), LiFe c Ni d Co e P.O. 4 , LiFe c Ni d Mn e P.O. 4 , LiNi c Co d Mn e P.O. 4 (c+d+e is 1 or less, 0<c<1, 0<d<1, 0<e<1), LiFe f Ni g Co h Mn i P.O. 4 (f+g+h+i is 1 or less, 0<f<1, 0<g<1, 0<h<1, 0<i<1), etc.
[0095] Furthermore, when the particle surface of the particulate first material 100x, which functions as a positive electrode active material, is almost entirely covered with the second material 100y, it is possible that charge / discharge characteristics different from those obtained when the first material 100x and the second material 100y are simply mixed together may be obtained.
[0096] The positive electrode of the present invention may have a structure in which at least a portion of the surface of a composite having a positive electrode active material is covered with a graphene compound. Preferably, the structure is such that 80% or more of the particle surfaces of the composite having the positive electrode active material and / or the aggregates having the composite are covered with the graphene compound. The graphene compound will be described later.
[0097] [Method 1 for Fabricating Positive Electrode] An example of a method for fabricating a positive electrode according to one embodiment of the present invention will be described with reference to FIGS. 6A and 6B.
[0098] In step S101 of FIG. 6A, the binder 110 is prepared, and in step S102, the dispersion medium 120 is prepared.
[0099] The binder 110 can be made of one or more of the following materials: polystyrene, methyl polyacrylate, methyl polymethacrylate (polymethyl methacrylate, PMMA), sodium polyacrylate, polyvinyl alcohol (PVA), polyethylene oxide (PEO), polypropylene oxide, polyimide, polyvinyl chloride, polytetrafluoroethylene, polyethylene, polypropylene, polyisobutylene, polyethylene terephthalate, nylon, polyvinylidene fluoride (PVDF), polyacrylonitrile (PAN), ethylene propylene diene polymer, polyvinyl acetate, nitrocellulose, and the like.
[0100] Polyimide has excellent thermal, mechanical, and chemical stability. Furthermore, when polyimide is used as a binder, a dehydration reaction and a cyclization (imidization) reaction occur. These reactions can be performed, for example, by heat treatment. In an electrode according to one embodiment of the present invention, when graphene having an oxygen-containing functional group is used as the graphene compound and polyimide is used as the binder, the graphene compound can also be reduced by the heat treatment, thereby simplifying the process. Furthermore, because polyimide has excellent heat resistance, the heat treatment can be performed at a heating temperature of, for example, 200° C. or higher. By performing the heat treatment at a heating temperature of 200° C. or higher, the reduction reaction of the graphene compound can be sufficiently performed, thereby further increasing the conductivity of the electrode.
[0101] A fluorine-containing polymer material, such as a fluoropolymer, can be used. PVDF is a resin with a melting point in the range of 134°C to 169°C, and is a material with excellent thermal stability.
[0102] As the binder, rubber materials such as styrene-butadiene rubber (SBR), styrene-isoprene-styrene rubber, acrylonitrile-butadiene rubber, butadiene rubber, ethylene-propylene-diene copolymer, etc. As the binder, fluororubber can be used.
[0103] Furthermore, it is preferable to use, for example, a water-soluble polymer as the binder. Examples of the water-soluble polymer that can be used include polysaccharides. Examples of the polysaccharide that can be used include cellulose derivatives such as carboxymethyl cellulose (CMC), methyl cellulose, ethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, and regenerated cellulose, as well as starch. It is even more preferable to use these water-soluble polymers in combination with the above-mentioned rubber material.
[0104] The binder may be used in combination with two or more of the above.
[0105] The dispersion medium 120 may be, for example, one or a mixture of two or more of water, methanol, ethanol, acetone, tetrahydrofuran (THF), dimethylformamide (DMF), N-methylpyrrolidone (NMP), and dimethyl sulfoxide (DMSO).
[0106] A suitable combination of the binder 110 and the dispersion medium 120 is preferably a combination of polyvinylidene fluoride (PVDF) and N-methylpyrrolidone (NMP).
[0107] Next, in step S103, the binder 110 and the dispersion medium 120 are mixed to obtain a binder mixture 1001 in step S104. For example, a propeller mixer, a planetary rotation mixer, or a thin film swirl mixer can be used as the mixing method. It is desirable that the binder mixture 1001 be in a state in which the binder 110 is well dispersed in the dispersion medium 120.
[0108] 6B, a binder mixture 1001 is prepared in step S111, and a conductive agent 1002 is prepared in step S112. In order to knead the mixture in a later step, the amount of binder mixture 1001 prepared in step S111 can be an amount smaller than the total amount required to form the positive electrode active material layer, and can be a mixing amount suitable for kneading. In this case, the shortage of binder mixture 1001 can be added in a step after kneading. Note that kneading refers to kneading with high viscosity.
[0109] As the conductive agent 1002, for example, one or more of the following can be used: carbon black such as acetylene black and furnace black; graphite such as artificial graphite and natural graphite; carbon fibers such as carbon nanofibers and carbon nanotubes; and graphene compounds.
[0110] In this specification and the like, graphene compounds refer to graphene, multilayer graphene, multi-graphene, graphene oxide, multilayer graphene oxide, multi-graphene oxide, reduced graphene oxide, reduced multilayer graphene oxide, reduced multi-graphene oxide, graphene quantum dots, etc. Graphene compounds contain carbon, have a shape such as a plate or sheet, and have a two-dimensional structure formed by six-membered carbon rings. The two-dimensional structure formed by six-membered carbon rings may also be referred to as a carbon sheet. Graphene compounds may have a functional group containing oxygen. Furthermore, graphene compounds preferably have a curved shape. Furthermore, graphene compounds may be rolled up to resemble carbon nanofibers.
[0111] In this specification and the like, graphene oxide refers to, for example, a material that contains carbon and oxygen, has a sheet-like shape, and has a functional group, in particular, an epoxy group, a carboxy group, or a hydroxy group.
[0112] In this specification, reduced graphene oxide refers to, for example, a material containing carbon and oxygen, having a sheet-like shape, and having a two-dimensional structure formed by six-membered carbon rings. It may also be called a carbon sheet. A single reduced graphene oxide can function, but multiple sheets may be stacked. Reduced graphene oxide preferably has a portion where the carbon concentration is greater than 80 atomic % and the oxygen concentration is 2 atomic % or more and 15 atomic % or less. By achieving these carbon and oxygen concentrations, reduced graphene oxide can function as a highly conductive agent even in small amounts. Furthermore, reduced graphene oxide preferably has an intensity ratio G / D between the G band and the D band in a Raman spectrum of 1 or more. Reduced graphene oxide with such an intensity ratio can function as a highly conductive agent even in small amounts.
[0113] By reducing graphene oxide, it may be possible to provide holes in the graphene compound.
[0114] Alternatively, a material in which the ends of graphene are terminated with fluorine may be used.
[0115] In the longitudinal section of the active material layer, the sheet-like graphene compound is dispersed substantially uniformly in the inner region of the active material layer. The plurality of graphene compounds are formed so as to partially cover the plurality of granular active material particles or to be attached to the surfaces of the plurality of granular active material particles, and are in surface contact with each other.
[0116] Here, a plurality of graphene compounds are bonded together to form a mesh-like graphene compound sheet (hereinafter referred to as a graphene compound net or graphene net). When an active material is covered with a graphene net, the graphene net can also function as a binder that binds the active materials together. Therefore, the amount of binder can be reduced or no binder can be used, thereby improving the ratio of the active material to the electrode volume and electrode weight. In other words, the charge / discharge capacity of a secondary battery can be increased.
[0117] Here, it is preferable to use graphene oxide as the graphene compound, mix it with an active material to form a layer that will become an active material layer, and then reduce it. That is, the completed active material layer preferably contains reduced graphene oxide. By using graphene oxide, which has extremely high dispersibility in a polar solvent, to form the graphene compound, it is possible to substantially uniformly disperse the graphene compound in the internal region of the active material layer. Since the solvent is volatilized and removed from the dispersion medium containing the uniformly dispersed graphene oxide and the graphene oxide is reduced, the graphene compound remaining in the active material layer partially overlaps and is dispersed to such an extent that it is in surface contact with each other, thereby forming a three-dimensional conductive path. Note that the reduction of graphene oxide may be performed, for example, by heat treatment or using a reducing agent.
[0118] Furthermore, by using a spray dryer in advance, a graphene compound, which is a conductive agent, can be formed as a coating that covers the entire surface of the active material, and further, the active material can be electrically connected to each other by the graphene compound to form a conductive path.
[0119] Furthermore, a material used in forming the graphene compound may be mixed with the graphene compound and used in the active material layer. For example, particles used as a catalyst in forming the graphene compound may be mixed with the graphene compound. Examples of catalysts used in forming the graphene compound include silicon oxide (SiO 2 , SiO x(x<2)), aluminum oxide, iron, nickel, ruthenium, iridium, platinum, copper, germanium, etc. The particles preferably have a D50 of 1 μm or less, more preferably 100 nm or less.
[0120] The graphene compound preferably has holes in parts of the carbon sheet. In the graphene compound, by providing holes in parts of the carbon sheet through which carrier ions such as lithium ions can pass, the insertion and desorption of carrier ions becomes easier on the surface of the active material covered with the graphene compound, and the rate characteristics of the secondary battery can be improved. The holes provided in parts of the carbon sheet may be called voids, defects, or gaps.
[0121] Next, in step S113, the binder mixture 1001 and the conductive agent 1002 are mixed to obtain a mixture 1010 in step S121. As a mixing method, for example, a propeller type mixer, a planetary rotation type mixer, or a thin film swirl type mixer can be used.
[0122] Next, in step S122 of FIG. 6B, a composite 100z having a positive electrode active material is prepared.
[0123] Next, in step S123, the mixture 1010 and the composite 100z having the positive electrode active material are mixed to obtain the mixture 1020 in step S131. For example, a propeller mixer, a planetary rotation mixer, or a thin film swirl mixer can be used as a mixing method. If the viscosity is appropriately adjusted in the mixing of step S123, the agglomeration of powder such as the positive electrode active material can be broken down by kneading.
[0124] Next, in step S132, a binder mixture 1001 is prepared, and in step S133, a dispersion medium 1003 is prepared. If, in step S111, an amount of binder mixture 1001 less than the total amount necessary to form the positive electrode active material layer is prepared, the shortage of binder mixture 1001 can be added in step S132. If the entire amount of binder mixture 1001 necessary to form the positive electrode active material layer is prepared in step S111, it is not necessary to prepare binder mixture 1001 in step S132. As the dispersion medium 1003, the same dispersion medium as in step S102 of FIG. 6A can be used. It is desirable to adjust the amount of dispersion medium 1003 to be prepared so that the viscosity is appropriate for application in a later step.
[0125] Next, in step S134, the mixture 1020 and dispersion medium 1003 from step S131 are mixed with the binder mixture 1001 prepared in step S132 to obtain a mixture 1030 from step S135. The mixture 1030 may be referred to as a positive electrode slurry.
[0126] Next, in step S136, the mixture 1030 is applied to a current collector. Highly conductive materials, such as metals such as stainless steel, gold, platinum, aluminum, and titanium, and alloys thereof, can be used as the current collector. It is preferable that the material used for the positive electrode current collector does not leach at the potential of the positive electrode. The materials described in embodiment 6 may also be used for the current collector. The application method in step S136 can be a slot die method, a gravure method, a blade method, or a combination thereof. A continuous coater or the like may also be used for application. Following step S136, in step S137, the mixture 1030 applied to the current collector is dried. Examples of drying methods that can be used include batch methods using a hot plate, a drying oven, a forced air drying oven, and a vacuum drying oven, as well as continuous methods combining hot air drying and infrared drying with a continuous coater.
[0127] Through the above steps, the positive electrode 2000 of one embodiment of the present invention can be manufactured (Step S140).
[0128] This embodiment mode can be implemented in appropriate combination with other embodiment modes.
[0129] Embodiment 2 In this embodiment, a method for manufacturing a positive electrode according to one embodiment of the present invention will be described.
[0130] The positive electrode includes a positive electrode active material layer and a positive electrode current collector. The positive electrode active material layer includes a first material 100x and a second material 100y that function as positive electrode active materials, and may further include a conductive agent and a binder.
[0131] The first material 100x can be made of any of the above-described materials and the materials described in Embodiments 3 and 4. The second material 100y can be made of any of the above-described materials and the materials described in Embodiment 5.
[0132] In this embodiment, examples of methods for fabricating a positive electrode having a first material 100x and a second material 100y are shown as positive electrode fabrication method 2, positive electrode fabrication method 3, and positive electrode fabrication method 4. A desirable form of the positive electrode is one in which the first material 100x and the second material 100y are well dispersed and have a good conductive network in the positive electrode active material layer. For example, a structure in which the amount of conductive agent in contact with one of the positive electrode active materials, which has low electronic conductivity, is greater than the amount of conductive agent in contact with the other positive electrode active material is desirable. Here, the amount of conductive agent in contact with the positive electrode active material can be considered as the coverage of the conductive agent on the particle surface of the positive electrode active material, and can be measured, for example, by surface SEM observation, cross-sectional SEM observation, or cross-sectional TEM observation.
[0133] In a positive electrode according to one embodiment of the present invention, a first material 100x and a second material 100y are mixed, and the first material 100x is LiMO. 2 (M1 is one or more selected from Fe, Ni, Co, Mn, and Al) is used as the second material 100y. 4When M2 is one or more selected from Fe, Ni, Co, and Mn, the higher the mixing ratio of the second material 100y, which has high stability at high temperatures and a stable crystal structure even in a high-voltage charging state, the higher the fire resistance and heat resistance of a secondary battery using the positive electrode of one embodiment of the present invention. Note that even when the ratio of the second material 100y is reduced, such as when the mixing ratio of the first material 100x:second material 100y is 7:3, 8:2, or 9:1, a secondary battery using the positive electrode of one embodiment of the present invention may still have fire resistance.
[0134] Positive electrode preparation method 2 shows an example of a positive electrode preparation method including a preparation step of mixing a first material 100x, a second material 100y, and a mixture of a conductive agent and a binder. Positive electrode preparation method 3 shows an example of a positive electrode preparation method including a first preparation step of mixing a first material 100x and a second material 100y, and a second preparation step of mixing the mixture obtained in the first step with a mixture of a conductive agent and a binder. Positive electrode preparation method 4 shows an example of a positive electrode preparation method including a first preparation step of mixing a second material 100y with a mixture of a conductive agent and a binder, and a second preparation step of mixing the mixture obtained in the first step with the first material 100x. However, the present invention should not be construed as being limited to these descriptions.
[0135] [Method 2 for Fabricating Positive Electrode] An example of a method for fabricating a positive electrode according to one embodiment of the present invention will be described with reference to FIGS. 7A and 7B.
[0136] 7A, a binder 110 is prepared in step S101, and a dispersion medium 120 is prepared in step S102. The materials shown in the first embodiment can be used for the binder 110 and the dispersion medium 120.
[0137] Next, in step S103, the binder 110 and the dispersion medium 120 are mixed to obtain a binder mixture 1001 in step S104. For example, a propeller mixer, a planetary rotation mixer, or a thin film swirl mixer can be used as the mixing method. It is desirable that the binder mixture 1001 be in a state in which the binder 110 is well dispersed in the dispersion medium 120.
[0138] 7B, a binder mixture 1001 is prepared in step S111, and a conductive agent 1002 is prepared in step S112. In order to knead the mixture in a later step, the amount of binder mixture 1001 prepared in step S111 can be an amount smaller than the total amount required to form the positive electrode active material layer, and can be a mixing amount suitable for kneading. In this case, the shortage of binder mixture 1001 can be added in a step after kneading. Note that kneading refers to kneading with high viscosity.
[0139] As the conductive agent 1002, for example, one or more of the following can be used: carbon black such as acetylene black and furnace black; graphite such as artificial graphite and natural graphite; carbon fibers such as carbon nanofibers and carbon nanotubes; and graphene compounds.
[0140] Next, in step S113, the binder mixture 1001 and the conductive agent 1002 are mixed to obtain a mixture 1010 in step S121. As a mixing method, for example, a propeller type mixer, a planetary rotation type mixer, or a thin film swirl type mixer can be used.
[0141] In step S122 of FIG. 7B, a first material 100x is prepared, and in step S123, a second material 100y is prepared.
[0142] The first material 100x and the second material 100y can be formed using the materials described in Embodiment 1.
[0143] As a combination of the first material 100x and the second material 100y, it is possible to select a combination that is less likely to cause a step in the charge / discharge curve, or a combination that causes a step in the charge / discharge curve at a desired charging rate, depending on the characteristics required of the secondary battery.
[0144] Next, in step S124, the mixture 1010, the first material 100x, and the second material 100y are mixed to obtain the mixture 1020 in step S131. For example, a propeller mixer, a planetary rotation mixer, or a thin film swirl mixer can be used as the mixing method in step S124. If the viscosity is appropriately adjusted in the mixing in step S124, the agglomeration of powder such as the positive electrode active material can be broken down by kneading.
[0145] Next, in step S132, a binder mixture 1001 is prepared, and in step S133, a dispersion medium 1003 is prepared. If, in step S111, an amount of binder mixture 1001 less than the total amount necessary to form the positive electrode active material layer is prepared, the shortage of binder mixture 1001 can be added in step S132. If the entire amount of binder mixture 1001 necessary to form the positive electrode active material layer is prepared in step S111, it is not necessary to prepare binder mixture 1001 in step S132. As the dispersion medium 1003, the same dispersion medium as in step S102 of FIG. 7A can be used. It is desirable to adjust the amount of dispersion medium 1003 to be prepared so that the viscosity is appropriate for application in a later step.
[0146] Next, in step S134, the mixture 1020 from step S131, the binder mixture 1001 prepared in step S132, and the dispersion medium 1003 prepared in step S133 are mixed together to obtain a mixture 1030 from step S135. The mixture 1030 may be referred to as a positive electrode slurry.
[0147] Next, in step S136, the mixture 1030 is applied to a current collector. The material described in Embodiment 1 can be used for the current collector. The application in step S136 and the drying in step S137 can be performed in the same manner as in steps S136 and S137 shown in FIG. 6 .
[0148] Through the above steps, the positive electrode 2000 of one embodiment of the present invention can be manufactured (Step S140).
[0149] [Method 3 for Fabricating Positive Electrode] Another example of a method for fabricating a positive electrode according to one embodiment of the present invention will be described with reference to FIGS.
[0150] In step S111 of FIG. 8, a binder mixture 1001 is prepared, and in step S112, a conductive agent 1002 is prepared. The binder mixture 1001 shown in FIG. 7A can be used as the binder mixture 1001. In order to knead the mixture in a later step, the amount of binder mixture 1001 prepared in step S111 can be an amount less than the total amount necessary to form the positive electrode active material layer, and can be a mixed amount suitable for kneading. In this case, the shortage of binder mixture 1001 can be added in a step after kneading. Note that kneading refers to kneading with high viscosity.
[0151] As the conductive agent 1002, for example, one or more of the following can be used: carbon black such as acetylene black and furnace black; graphite such as artificial graphite and natural graphite; carbon fibers such as carbon nanofibers and carbon nanotubes; and graphene compounds.
[0152] Next, in step S113, the binder mixture 1001 and the conductive agent 1002 are mixed to obtain a mixture 1010 in step S121. As a mixing method, for example, a propeller type mixer, a planetary rotation type mixer, or a thin film swirl type mixer can be used.
[0153] In step S131 of FIG. 8, a first material 100x is prepared, and in step S132, a second material 100y is prepared.
[0154] The first material 100x and the second material 100y can be formed using the materials described in Embodiment 1.
[0155] As a combination of the first material 100x and the second material 100y, it is possible to select a combination that is less likely to cause a step in the charge / discharge curve, or a combination that causes a step in the charge / discharge curve at a desired charging rate, depending on the characteristics required of the secondary battery.
[0156] Next, in step S133, the first material 100x and the second material 100y are mixed to obtain a mixture 1100 in step S141. As a mixing method, for example, a ball mill, a propeller mixer, a planetary rotation mixer, or a thin film swirl mixer can be used.
[0157] Next, in step S142, mixture 1010 from step S121 and mixture 1100 from step S141 are mixed to obtain mixture 1020 from step S151. For example, a propeller mixer, a planetary rotation mixer, or a thin film swirl mixer can be used as the mixing method. If the viscosity is appropriately adjusted during the mixing in step S142, agglomerations of powder such as the positive electrode active material can be loosened by kneading.
[0158] Next, in step S152, a binder mixture 1001 is prepared, and in step S153, a dispersion medium 1003 is prepared. If, in step S111, an amount of binder mixture 1001 less than the total amount necessary to form the positive electrode active material layer is prepared, the shortage of binder mixture 1001 can be added in step S152. If the entire amount of binder mixture 1001 necessary to form the positive electrode active material layer is prepared in step S111, it is not necessary to prepare binder mixture 1001 in step S152. As the dispersion medium 1003, the same dispersion medium as in step S102 of FIG. 7A can be used. It is desirable to adjust the amount of dispersion medium 1003 to be prepared so that the viscosity is appropriate for application in a later step.
[0159] Next, in step S154, the mixture 1020 from step S151, the binder mixture 1001 prepared in step S152, and the dispersion medium 1003 prepared in step S153 are mixed together to obtain a mixture 1030 from step S155. The mixture 1030 may be referred to as a positive electrode slurry.
[0160] Next, in step S156, the mixture 1030 is applied to a current collector. The material described in Embodiment 1 can be used for the current collector. The application in step S156 and the drying in step S157 can be performed in the same manner as in steps S136 and S137 shown in FIG. 6 .
[0161] Through the above steps, the positive electrode 2000 of one embodiment of the present invention can be manufactured (Step S160).
[0162] [Method 4 for Fabricating Positive Electrode] Another example of a method for fabricating a positive electrode according to one embodiment of the present invention will be described with reference to FIGS.
[0163] In step S111 of FIG. 9, a binder mixture 1001 is prepared, and in step S112, a conductive agent 1002 is prepared. The binder mixture 1001 shown in FIG. 7A can be used as the binder mixture 1001. In order to knead the mixture in a later step, the amount of binder mixture 1001 prepared in step S111 can be an amount less than the total amount necessary to form the positive electrode active material layer, and can be a mixed amount suitable for kneading. In this case, the shortage of binder mixture 1001 can be added in a step after kneading. Note that kneading refers to kneading with high viscosity.
[0164] As the conductive agent 1002, for example, one or more of the following can be used: carbon black such as acetylene black and furnace black; graphite such as artificial graphite and natural graphite; carbon fibers such as carbon nanofibers and carbon nanotubes; and graphene compounds.
[0165] Next, in step S113, the binder mixture 1001 and the conductive agent 1002 are mixed to obtain a mixture 1010 in step S121. As a mixing method, for example, a propeller type mixer, a planetary rotation type mixer, or a thin film swirl type mixer can be used.
[0166] Next, in step S122 of FIG. 9, a second material 100y is prepared.
[0167] The second material 100y is LiMPO having an olivine-type crystal structure, which is produced by the production method shown in the fifth embodiment described later. 4 (M2 is one or more selected from Fe, Ni, Co, and Mn). 4 Materials such as those mentioned above as LiFePO 4 , LiMnPO 4 , LiFe a Mn b P.O. 4 (a+b is 1 or less, 0<a<1, 0<b<1), LiFe a Ni b P.O. 4 (a+b is 1 or less, 0<a<1, 0<b<1) can be used. Furthermore, the particle surfaces of the second material 100y may have a carbon coating layer.
[0168] Next, in step S123, the mixture 1010 and the second material 100y are mixed to obtain a mixture 1021 in step S131. For example, a propeller mixer, a planetary rotation mixer, or a thin film swirl mixer can be used as the mixing method. When the viscosity is appropriately adjusted in the mixing of step S123, the agglomeration of powder such as the positive electrode active material can be broken down by kneading.
[0169] In the process of fabricating a positive electrode having a first material 100x and a second material 100y, if the second material 100y has lower electronic conductivity than the first material 100x, it is desirable to mix the second material 100y with a conductive agent before mixing the first material 100x, which makes it possible to obtain a structure in which the amount of conductive agent in contact with the second material 100y is greater than the amount of conductive agent in contact with the first material 100x.
[0170] Next, in step S132, a first material 100x is prepared.
[0171] The first material 100x and the second material 100y can be formed using the materials described in Embodiment 1.
[0172] As a combination of the first material 100x and the second material 100y, it is possible to select a combination that is less likely to cause a step in the charge / discharge curve, or a combination that causes a step in the charge / discharge curve at a desired charging rate, depending on the characteristics required of the secondary battery.
[0173] Next, in step S142, the mixture 1021 and the first material 100x are mixed to obtain the mixture 1022 in step S151. For example, a propeller mixer, a planetary rotation mixer, or a thin film swirl mixer can be used as the mixing method. When the viscosity is appropriately adjusted in the mixing in step S142, the agglomeration of powder such as the positive electrode active material can be loosened by kneading.
[0174] Next, in step S152, a binder mixture 1001 is prepared, and in step S153, a dispersion medium 1003 is prepared. If, in step S111, an amount of binder mixture 1001 less than the total amount necessary to form the positive electrode active material layer is prepared, the shortage of binder mixture 1001 can be added in step S152. If the entire amount of binder mixture 1001 necessary to form the positive electrode active material layer is prepared in step S111, it is not necessary to prepare binder mixture 1001 in step S152. As the dispersion medium 1003, the same dispersion medium as in step S102 of FIG. 7A can be used. It is desirable to adjust the amount of dispersion medium 1003 to be prepared so that the viscosity is appropriate for application in a later step.
[0175] Next, in step S154, the mixture 1022 from step S151, the binder mixture 1001 prepared in step S152, and the dispersion medium 1003 prepared in step S153 are mixed together to obtain a mixture 1030 from step S155. The mixture 1030 may be referred to as a positive electrode slurry.
[0176] Next, in step S156, the mixture 1030 is applied to a current collector. The material described in Embodiment 1 can be used for the current collector. The application in step S156 and the drying in step S157 can be performed in the same manner as in steps S136 and S137 shown in FIG. 6 .
[0177] Through the above steps, the positive electrode 2000 of one embodiment of the present invention can be manufactured (Step S160).
[0178] This embodiment mode can be implemented in appropriate combination with other embodiment modes.
[0179] In this embodiment, an example of a method for manufacturing a positive electrode active material of one embodiment of the present invention will be described with reference to FIGS. 10A to 16C. In addition, the positive electrode active material of one embodiment of the present invention will be described with reference to FIGS. 17A to 25C.
[0180] [Method 1 for Manufacturing Positive Electrode Active Material] An example of a method for manufacturing a positive electrode active material according to one embodiment of the present invention will be described with reference to FIGS. 10A and 10B.
[0181] 10A, a lithium source and a transition metal source are prepared as materials for lithium and transition metal. Note that in the drawing, the transition metal source is illustrated as an M1 source.
[0182] As the lithium source, for example, lithium carbonate, lithium fluoride, etc. can be used.
[0183] The transition metal source may be, for example, at least one of manganese, cobalt, and nickel. For example, the transition metal source may be a combination of cobalt alone, nickel alone, cobalt and manganese, cobalt and nickel, or cobalt, manganese, and nickel.
[0184] It is preferable to use a high-purity material as the transition metal source used in the synthesis. Specifically, the purity of the material is 3N (99.9%) or higher, preferably 4N (99.99%) or higher, more preferably 4N (99.995%) or higher, and even more preferably 5N (99.999%) or higher. The use of a high-purity material can increase the capacity and / or reliability of the secondary battery.
[0185] In addition, it is preferable that the transition metal source has high crystallinity. For example, it is preferable that the transition metal source has single crystal grains. The crystallinity of the transition metal source can be evaluated, for example, from a TEM (transmission electron microscope) image, a STEM (scanning transmission electron microscope) image, a HAADF-STEM (high-angle annular dark-field scanning transmission electron microscope) image, an ABF-STEM (annular bright-field scanning transmission electron microscope) image, etc. Furthermore, X-ray diffraction (XRD), electron diffraction, neutron diffraction, etc. can also be used to evaluate the crystallinity of the transition metal source. Note that the above-mentioned crystallinity evaluation can be applied not only to the transition metal source, but also to the evaluation of the crystallinity of primary particles or secondary particles.
[0186] Furthermore, when using metals capable of forming a layered rock-salt type composite oxide, it is preferable to set the mixing ratio of cobalt, manganese, and nickel within a range that allows a layered rock-salt type crystal structure to be formed. Furthermore, an additional element X may be added to these transition metals within a range that allows a layered rock-salt type crystal structure to be formed. An example of the process of adding the additional element X is shown in FIG. 10B. In step S11, a lithium source, a transition metal source, and an additional element X source are prepared, and then step S12 is performed.
[0187] The additive element X source can be one or more selected from nickel, cobalt, magnesium, calcium, chlorine, fluorine, aluminum, manganese, titanium, zirconium, yttrium, vanadium, iron, chromium, niobium, lanthanum, hafnium, zinc, silicon, sulfur, phosphorus, boron, and arsenic. Bromine and beryllium may also be used as the additive element X source in addition to the above elements. However, since bromine and beryllium are toxic to living organisms, it is preferable to use the additive element X source described above.
[0188] The transition metal source may be an oxide or hydroxide of the metals exemplified above, and the cobalt source may be, for example, cobalt oxide or cobalt hydroxide.
[0189] As the manganese source, manganese oxide, manganese hydroxide, etc. can be used. As the nickel source, nickel oxide, nickel hydroxide, etc. can be used. As the aluminum source, aluminum oxide, aluminum hydroxide, etc. can be used.
[0190] <Step S12> Next, in step S12, the lithium source and transition metal source are crushed and mixed. Crushing and mixing can be performed by dry or wet methods. It is particularly preferable to perform crushing using dehydrated acetone with a purity of 99.5% or higher, in which the water content is reduced to 10 ppm or less. Note that, in this specification, the term "crushing" may be interpreted as "pulverization." Mixing can be performed using, for example, a ball mill or a bead mill. When using a ball mill, it is preferable to use zirconia balls as the media. When using a ball mill or a bead mill, it is preferable to set the peripheral speed to 100 mm / s or more and 2000 mm / s or less to suppress contamination from the media or materials. Note that step S12 is performed at a peripheral speed of 838 mm / s (rotation speed: 400 rpm, diameter of ball mill container: 40 mm). Furthermore, using the dehydrated acetone described above in crushing and mixing can reduce impurities that may be mixed into the materials.
[0191] <Step S13> Next, in step S13, the mixed materials are heated. The heating temperature in this step is preferably 800°C or higher and lower than 1100°C, more preferably 900°C or higher and 1000°C or lower, and even more preferably about 950°C. If the temperature is too low, the decomposition and melting of the lithium source and transition metal source may be insufficient. On the other hand, if the temperature is too high, defects may occur due to factors such as lithium transpiration from the lithium source and / or excessive reduction of the metal used as the transition metal source. For example, when cobalt is used as the transition metal, defects may occur in which cobalt becomes divalent.
[0192] The heating time can be, for example, 1 hour or more and 100 hours or less, and preferably 2 hours or more and 20 hours or less. The heating is preferably carried out in an atmosphere with little water, such as dry air (for example, a dew point of -50°C or less, more preferably a dew point of -80°C or less). In this embodiment, the heating is carried out in an atmosphere with a dew point of -93°C. The heating is carried out in a CH 4 , CO, CO 2 , and H 2 It is preferable to perform the treatment in an atmosphere in which the impurity concentrations of the above are 5 ppb (parts per billion) or less, since this can suppress impurities that may be mixed into the material.
[0193] For example, when heating at 1000°C for 10 hours, it is preferable to increase the temperature by 200°C / h and to supply dry air at a flow rate of 10 L / min. The heated material can then be cooled to room temperature. For example, it is preferable to set the cooling time from the specified temperature to room temperature to 10 hours or more and 50 hours or less. However, cooling to room temperature in step S13 is not essential.
[0194] The crucible or sheath used in the heating step S13 is preferably made of a highly heat-resistant material such as alumina (aluminum oxide), mullite / cordierite, magnesia, or zirconia. An alumina crucible is preferable because it is a material that does not contain impurities. In this embodiment, an alumina crucible with a purity of 99.9% is preferably used. It is preferable to heat the crucible or sheath with a lid, which prevents the material from volatilizing.
[0195] Furthermore, when recovering the material after heating in step S13, it is preferable to transfer the material from the crucible to a mortar and then recover it, since this prevents impurities from being mixed into the material. It is also preferable that the mortar be made of a material that does not allow impurities to be mixed in. Specifically, it is preferable to use a mortar made of alumina with a purity of 90% or more, preferably 99% or more. Note that conditions equivalent to those of step S13 can also be applied to heating steps other than step S13, which will be described later.
[0196] 10A and 10B, the positive electrode active material 100A and the positive electrode active material 100B of one embodiment of the present invention can be manufactured (Step S14). The positive electrode active material 100A and the positive electrode active material 100B can be used as the first material 100x described in Embodiments 1 and 2.
[0197] [Method 2 for Manufacturing Positive Electrode Active Material] Next, another example of a method for manufacturing a positive electrode active material of one embodiment of the present invention will be described with reference to FIGS. 11A, 11B, and 11C.
[0198] In FIG. 11A, steps S11 to S14 are performed in the same manner as in FIG. 10A to obtain a composite oxide containing lithium, a transition metal, and oxygen (LiMO 2 ) to prepare.
[0199] It is also possible to use a pre-synthesized composite oxide in step S14. In this case, steps S11 to S13 can be omitted. When preparing a pre-synthesized composite oxide, it is preferable to use a high-purity material. The purity of the material is 99.5% or more, preferably 99.9% or more, and more preferably 99.99% or more.
[0200] <Step S20> In step S20 of Fig. 11A, an additive element X source is prepared. The materials described above can be used as the additive element X source. Furthermore, a plurality of elements may be used as the additive element X. A case in which a plurality of elements are used as the additive element X will be described with reference to Figs. 11B and 11C.
[0201] 11B, a magnesium source (Mg source) and a fluorine source (F source) are prepared. A lithium source may also be prepared in addition to the magnesium source and the fluorine source.
[0202] As the magnesium source, for example, magnesium fluoride, magnesium oxide, magnesium hydroxide, magnesium carbonate, etc. can be used.
[0203] Examples of fluorine sources include lithium fluoride (LiF) and magnesium fluoride (MgF 2 ), aluminum fluoride (AlF 3 ), titanium fluoride (TiF 4 ), cobalt fluoride (CoF 2 , CoF 3 ), nickel fluoride (NiF 2 ), zirconium fluoride (ZrF 4 ), vanadium fluoride (VF 5 ), manganese fluoride, iron fluoride, chromium fluoride, niobium fluoride, zinc fluoride (ZnF 2 ), calcium fluoride (CaF 2 ), sodium fluoride (NaF), potassium fluoride (KF), barium fluoride (BaF 2 ), cerium fluoride (CeF 2 ), lanthanum fluoride (LaF 3), sodium aluminum hexafluoride (Na 3 AlF 6 The fluorine source is not limited to a solid, and may be, for example, fluorine (F 2 ), fluorocarbon, sulfur fluoride, oxygen fluoride (OF 2 , O 2 F 2 , O 3 F 2 , O 4 F 2 , O 2 F), etc., may be used and mixed into the atmosphere in the heating step described below. A mixture of multiple fluorine sources may also be used. Among these, lithium fluoride is preferred because it has a relatively low melting point of 848°C and is easily melted in the heating step described below.
[0204] Examples of lithium sources that can be used include lithium fluoride and lithium carbonate. That is, lithium fluoride can be used as both a lithium source and a fluorine source. Magnesium fluoride can be used as both a fluorine source and a magnesium source.
[0205] In this embodiment, lithium fluoride (LiF) is prepared as the fluorine source, and magnesium fluoride (MgF) is prepared as the fluorine source and magnesium source. 2 Lithium fluoride (LiF) and magnesium fluoride (MgF) 2 is LiF:MgF 2 Mixing lithium fluoride (LiF) and magnesium fluoride (MgF) in a molar ratio of about 65:35 results in the greatest effect of lowering the melting point (Non-Patent Document 4). On the other hand, if the amount of lithium fluoride is too high, there is a concern that the lithium will be excessive and the cycle characteristics will deteriorate. Therefore, 2 The molar ratio of LiF:MgF 2 =x:1 (0≦x≦1.9), and LiF:MgF 2 =x:1 (0.1≦x≦0.5) is more preferable, and LiF:MgF 2 = x: 1 (x = near 0.33) is more preferable. In this specification, "near" refers to a value that is greater than 0.9 times and smaller than 1.1 times the value.
[0206] Furthermore, if the subsequent mixing and crushing steps are performed wet, a solvent is prepared. Examples of solvents that can be used include ketones such as acetone, alcohols such as ethanol and isopropanol, ether, dioxane, acetonitrile, and N-methyl-2-pyrrolidone (NMP). It is more preferable to use an aprotic solvent that is less likely to react with lithium. In this embodiment, dehydrated acetone with a purity of 99.5% or higher is used.
[0207] <Step S22> Next, in step S22 of FIG. 11B, the above materials are mixed and crushed. Mixing can be performed by either a dry method or a wet method, but a wet method is preferred because it allows for smaller crushing. For example, a ball mill or a bead mill can be used for mixing. When using a ball mill, it is preferable to use zirconia balls as the media. The conditions for the ball mill or bead mill can be the same as those for step S12.
[0208] <Step S23> Next, in step S23, the crushed and mixed material is recovered to obtain a source of the additional element X. Note that the source of the additional element X shown in step S23 may be called a mixture because it is formed from a plurality of materials.
[0209] The mixture preferably has a D50 (median diameter) of 600 nm or more and 20 μm or less, and more preferably 1 μm or more and 10 μm or less. Such a finely pulverized mixture facilitates uniform adhesion of the mixture to the surface of the composite oxide particles when mixed with a composite oxide containing lithium, a transition metal, and oxygen in a subsequent process. Uniform adhesion of the mixture to the surface of the composite oxide particles is preferred because it facilitates thorough distribution of halogen and magnesium near the surface of the composite oxide particles after heating. If there are regions near the surface that do not contain halogen and magnesium, the O3'-type crystal structure described below may be difficult to achieve in a charged state.
[0210] 11B illustrates a method of mixing two materials, but is not limited to this. For example, as shown in FIG. 11C , four materials (a magnesium source (Mg source), a fluorine source (F source), a nickel source (Ni source), and an aluminum source (Al source)) may be mixed to prepare the additive element X source. Alternatively, the additive element X source may be prepared using a single material, i.e., one type of material. Nickel oxide, nickel hydroxide, etc. may be used as the nickel source. Aluminum oxide, aluminum hydroxide, etc. may be used as the aluminum source.
[0211] <Step S31> Next, in step S31 of FIG. 11A, the LiMO obtained in step S14 is 2 and a source of the additional element X. The ratio of the number of transition metal atoms M in the composite oxide containing lithium, transition metal, and oxygen to the number of magnesium atoms Mg in the additional element X is preferably M:Mg=100:y (0.1≦y≦6), and more preferably M:Mg=100:y (0.3≦y≦3).
[0212] The mixing conditions in step S31 are preferably milder than those in step S12 so as not to destroy the composite oxide particles. For example, it is preferable to use conditions with a lower rotation speed or a shorter time than those in step S12. It can also be said that dry mixing provides milder conditions than wet mixing. For example, a ball mill, a bead mill, or the like can be used for mixing. When using a ball mill, it is preferable to use zirconia balls as the media.
[0213] Here, dry mixing is performed in a ball mill using zirconia balls with a diameter of 1 mm at 150 rpm for 1 hour in a dry room with a dew point of −100° C. or higher and −10° C. or lower.
[0214] <Step S32> Next, in step S32 of FIG. 11A, the mixed materials are collected to obtain a mixture 903.
[0215] Although this embodiment describes a method of adding a mixture of lithium fluoride and magnesium fluoride to lithium cobalt oxide with few impurities, one embodiment of the present invention is not limited thereto. Instead of the mixture 903 in step S32, a starting material for lithium cobalt oxide to which a magnesium source, a fluorine source, and the like have been added and heated may be used. In this case, there is no need to separate the steps S11 to S14 from the steps S21 to S23, which simplifies the process and increases productivity.
[0216] Alternatively, lithium cobalt oxide to which magnesium and fluorine have been added in advance may be used. If lithium cobalt oxide to which magnesium and fluorine have been added is used, the steps up to step S32 can be omitted, which is simpler.
[0217] Alternatively, a magnesium source and a fluorine source may be further added to lithium cobalt oxide to which magnesium and fluorine have been added in advance.
[0218] <Step S33> Next, in step S33, the mixture 903 is heated in an atmosphere containing oxygen. The heating is preferably performed in such a manner that the particles of the mixture 903 do not stick to each other.
[0219] If the particles of the mixture 903 stick together during heating, the distribution of the additive elements, which are preferably distributed near the surface as described below, may deteriorate. Furthermore, the surface of the particles, which is preferably smooth and has few irregularities, may become more irregular if the particles stick together, which may increase defects such as cracks and / or fissures. This is thought to be due to the fact that the adhesion of the mixture 903 to each other reduces the contact area with oxygen in the atmosphere and blocks the route for the additive elements to diffuse.
[0220] The heating in step S33 may be performed using a rotary kiln. The heating in a rotary kiln may be performed while stirring, whether it is a continuous or batch type. The heating in step S33 may be performed using a roller hearth kiln.
[0221] The heating temperature in step S33 is LiMO2 The temperature at which the reaction between LiMO and the source of the added element X proceeds must be equal to or higher than the temperature at which the reaction proceeds. 2 The temperature may be lower than the melting point of these materials. For example, in the case of oxides, the melting point T m 0.757 times (Tammann temperature T d Therefore, the heating temperature in step S33 may be, for example, 500° C. or higher.
[0222] However, if the temperature is equal to or higher than the temperature at which at least a part of the mixture 903 melts, the reaction proceeds more easily, which is preferable. For example, LiF and MgF are used as the source of the additive element X. 2 When LiF and MgF 2 Since the eutectic point of is around 742°C, it is preferable to set the heating temperature in step S33 to 742°C or higher.
[0223] Also, LiCoO 2 :LiF:MgF 2 In the mixture 903 in which the molar ratio is 100:0.33:1, an endothermic peak is observed around 830° C. in differential scanning calorimetry (DSC measurement). Therefore, the heating temperature is preferably 830° C. or higher.
[0224] A higher heating temperature is preferable because the reaction proceeds more easily, the heating time is shorter, and productivity is higher.
[0225] However, the heating temperature is LiMO 2 Decomposition temperature of LiCoO 2 In addition, at temperatures close to the decomposition temperature, a small amount of LiMO 2 Therefore, the heating temperature in step S33 is preferably 1130° C. or less, more preferably 1000° C. or less, even more preferably 950° C. or less, and even more preferably 900° C. or less.
[0226] Therefore, the heating temperature in step S33 is preferably 500°C or higher and 1130°C or lower, more preferably 500°C or higher and 1000°C or lower, even more preferably 500°C or higher and 950°C or lower, and even more preferably 500°C or higher and 900°C or lower. Also, the heating temperature is preferably 742°C or higher and 1130°C or lower, more preferably 742°C or higher and 1000°C or lower, even more preferably 742°C or higher and 950°C or lower, and even more preferably 742°C or higher and 900°C or lower. Also, the heating temperature is preferably 830°C or higher and 1130°C or lower, more preferably 830°C or higher and 1000°C or lower, even more preferably 830°C or higher and 950°C or lower, and even more preferably 830°C or higher and 900°C or lower.
[0227] Furthermore, when the mixture 903 is heated, it is preferable to control the partial pressure of fluorine or fluoride in the atmosphere within an appropriate range.
[0228] In the manufacturing method described in this embodiment, some materials, for example, LiF, which is a fluorine source, may function as a flux. 2 The temperature can be lowered to a temperature lower than the decomposition temperature of the compound, for example, 742° C. to 950° C., and additive elements such as magnesium can be distributed near the surface, making it possible to produce a positive electrode active material with good characteristics.
[0229] However, since LiF has a lower specific gravity in a gaseous state than oxygen, the gaseous LiF easily escapes from the top of the heating vessel. Therefore, when LiF volatilizes due to heating, the amount of LiF in the mixture 903 decreases. This weakens the function as a flux. Therefore, it is necessary to heat while suppressing the volatilization of LiF. Even if LiF is not used as a fluorine source, etc., LiM1O 2 There is also a possibility that Li and F on the surface may react to produce LiF, which may then volatilize. Therefore, even if a fluoride with a higher melting point than LiF is used, it is still necessary to suppress volatilization.
[0230] Therefore, it is preferable to heat the mixture 903 in an atmosphere containing LiF, that is, to heat the mixture 903 in a state where the partial pressure of LiF is high in the heating furnace. By heating in this manner, it is possible to suppress the volatilization of LiF in the mixture 903.
[0231] Furthermore, when heating in a rotary kiln, it is preferable to control the flow rate of the oxygen-containing atmosphere in the kiln to heat the mixture 903. For example, it is preferable to reduce the flow rate of the oxygen-containing atmosphere, or to first purge the atmosphere and then not flow the atmosphere after introducing the oxygen atmosphere into the kiln.
[0232] When heating is performed using a roller hearth kiln, the mixture 903 can be heated in an atmosphere containing LiF by, for example, placing a lid on a container containing the mixture 903 .
[0233] The heating time is preferably determined by the heating temperature, the amount of LiM1O in step S14, and the like. 2 The temperature and time required for the reaction may vary depending on the particle size, composition, etc. Small particles may be more suitable at lower temperatures or for shorter times than large particles.
[0234] For example, when the average particle size (D50) of the composite oxide in step S14 of Fig. 11A is about 12 µm, the heating temperature is preferably, for example, 600°C or higher and 950°C or lower. The heating time is, for example, preferably 3 hours or longer, more preferably 10 hours or longer, and even more preferably 60 hours or longer.
[0235] On the other hand, when the average particle size (D50) of the composite oxide in step S14 is about 5 μm, the heating temperature is preferably, for example, 600° C. or higher and 950° C. or lower. The heating time is preferably, for example, 1 hour or higher and 10 hours or lower, and more preferably about 2 hours. The temperature-lowering time after heating is preferably, for example, 10 hours or higher and 50 hours or lower.
[0236] <Step S34> Next, the heated material is recovered to produce the positive electrode active material 100C. At this time, the recovered particles are preferably sieved. Through the above steps, the positive electrode active material 100C of one embodiment of the present invention can be produced (Step S34). The positive electrode active material 100C can be used as the first material 100x described in Embodiments 1 and 2.
[0237] [Method 3 for Manufacturing Positive Electrode Active Material] Next, another example of a method for manufacturing a positive electrode active material of one embodiment of the present invention will be described with reference to FIG. 12, and FIGS. 13A, 13B, and 13C.
[0238] 12, steps S11 to S14 are performed in the same manner as in FIG. 10A to obtain a composite oxide containing lithium, a transition metal, and oxygen (LiMO 2 ) to prepare.
[0239] Alternatively, a composite oxide containing lithium, a transition metal, and oxygen that has been synthesized in advance may be used in step S14, in which case steps S11 to S13 can be omitted.
[0240] <Step S20a> In step S20a of FIG. 12, a source of the additive element X1 is prepared. The source of the additive element X1 can be selected from the additive elements X described above. For example, one or more selected from magnesium, fluorine, and calcium can be suitably used as the additive element X1. In this embodiment, FIG. 13A illustrates a configuration in which magnesium and fluorine are used as the additive element X1. Steps S21 and S22 included in step S20a shown in FIG. 13A can be fabricated by the same processes as steps S21 and S22 shown in FIG. 11B.
[0241] Step S23 shown in FIG. 13A is a process of recovering the material crushed and mixed in step S22 shown in FIG. 13A to provide a source of the additional element X1.
[0242] 11. Steps S31 to S33 shown in FIG. 12 can be fabricated in the same manner as steps S31 to S33 shown in FIG.
[0243] <Step S34a> Next, the material heated in step S33 is recovered to produce a composite oxide.
[0244] <Step S40> In step S40 of FIG. 12, a source of the additive element X2 is prepared. The source of the additive element X2 can be selected from the additive elements X described above. For example, one or more selected from nickel, titanium, boron, zirconium, and aluminum can be suitably used as the additive element X2. In this embodiment, FIG. 13B illustrates a configuration in which nickel and aluminum are used as the additive element X2. Steps S41 and S42 included in step S40 shown in FIG. 13B can be fabricated using the same processes as steps S21 and S22 shown in FIG. 11B.
[0245] Step S43 shown in FIG. 13B is a process of recovering the material crushed and mixed in step S42 shown in FIG. 13B to provide a source of the additional element X2.
[0246] Step S40 shown in Fig. 13C is a modified example of step S40 shown in Fig. 13B. In Fig. 13C, a nickel source and an aluminum source are prepared (step S41), and each is independently crushed (step S42a), thereby preparing a plurality of sources of the additional element X2 (step S43).
[0247] <Steps S51 to S53> Next, step S51 in FIG. 12 is a step of mixing the composite oxide prepared in step S34a with the additive element X2 source prepared in step S40. Note that step S51 in FIG. 12 can be performed in a manner similar to step S31 shown in FIG. 11A. Also, step S52 in FIG. 12 can be performed in a manner similar to step S32 shown in FIG. 11A. Note that the material prepared in step S52 in FIG. 12 is mixture 904. Mixture 904 is a material that contains the additive element X2 source added in step S40 in addition to the material of mixture 903. Also, step S53 in FIG. 12 can be performed in a manner similar to step S33 shown in FIG. 11A.
[0248] <Step S54> Next, the heated material is recovered to produce the positive electrode active material 100D. At this time, the recovered particles are preferably sieved. Through the above steps, the positive electrode active material 100D of one embodiment of the present invention can be produced (Step S54). The positive electrode active material 100D can be used as the first material 100x described in Embodiment 1 and Embodiment 2.
[0249] As shown in Figure 12 and Figures 13A to 13C, by separating the steps of introducing the transition metal, the additional element X1, and the additional element X2, it may be possible to change the depth profile of each element. For example, the concentration of the additional element can be increased near the surface compared to the interior of the particle. Furthermore, using the number of transition metal atoms as a reference, the ratio of the number of additional element atoms to this reference can be made higher near the surface than in the interior.
[0250] [Method 4 for Producing Positive Electrode Active Material] <Step S11> In step S11 shown in FIG. 14A, a lithium source (Li source) and a transition metal source (M source) are prepared as starting materials for lithium and transition metal, respectively.
[0251] As the lithium source, it is preferable to use a compound containing lithium, such as lithium carbonate, lithium hydroxide, lithium nitrate, or lithium fluoride. It is preferable that the lithium source has high purity, and it is preferable to use a material with a purity of, for example, 99.99% or higher.
[0252] The transition metal can be selected from elements in Groups 4 to 13 of the periodic table, and for example, at least one of manganese, cobalt, and nickel is used. The transition metal may be only cobalt, only nickel, two elements (cobalt and manganese), two elements (cobalt and nickel), or three elements (cobalt, manganese, and nickel). When only cobalt is used, the resulting positive electrode active material has lithium cobalt oxide (LCO), and when three elements (cobalt, manganese, and nickel) are used, the resulting positive electrode active material has lithium nickel-cobalt-manganese oxide (NCM).
[0253] As the transition metal source, it is preferable to use a compound containing the above transition metal, and for example, an oxide or hydroxide of the metal exemplified as the above transition metal can be used. As a cobalt source, cobalt oxide, cobalt hydroxide, etc. can be used. As a manganese source, manganese oxide, manganese hydroxide, etc. can be used. As a nickel source, nickel oxide, nickel hydroxide, etc. can be used. As an aluminum source, aluminum oxide, aluminum hydroxide, etc. can be used.
[0254] The transition metal source preferably has a high purity, for example, a material with a purity of 3N (99.9%) or higher, preferably 4N (99.99%) or higher, more preferably 4N (99.995%) or higher, and even more preferably 5N (99.999%) or higher. By using a high-purity material, impurities in the positive electrode active material can be controlled. As a result, the capacity of the secondary battery is increased and / or the reliability of the secondary battery is improved.
[0255] Additionally, the transition metal source preferably has high crystallinity, for example, single crystal grains.
[0256] When two or more transition metal sources are used, the two or more transition metal sources are preferably prepared in a ratio (mixing ratio) that allows the two or more transition metal sources to form a layered rock salt type crystal structure.
[0257] <Step S12> Next, in step S12 shown in FIG. 14A, the lithium source and the transition metal source are crushed and mixed to prepare a mixed material. Crushing and mixing can be performed by either a dry or wet method. The wet method is preferred because it allows for smaller crushing. When performing the wet method, a solvent is prepared. Examples of solvents that can be used include ketones such as acetone, alcohols such as ethanol and isopropanol, ether, dioxane, acetonitrile, and N-methyl-2-pyrrolidone (NMP). It is more preferable to use an aprotic solvent that is less likely to react with lithium. In this embodiment, dehydrated acetone with a purity of 99.5% or higher is used. It is preferable to mix the lithium source and the transition metal source in dehydrated acetone with a purity of 99.5% or higher, with a water content reduced to 10 ppm or less, and then crush and mix the mixture. Using dehydrated acetone with the above purity can reduce potential impurities.
[0258] A ball mill, a bead mill, or the like can be used as a means for mixing, etc. When using a ball mill, it is preferable to use alumina balls or zirconia balls as grinding media. Zirconia balls are preferable because they emit less impurities. Furthermore, when using a ball mill, a bead mill, or the like, it is preferable to set the peripheral speed to 100 mm / s or more and 2000 mm / s or less in order to suppress contamination from the media. In this embodiment, the peripheral speed is set to 838 mm / s (rotation speed 400 rpm, diameter of ball mill container 40 mm).
[0259] <Step S13> Next, in step S13 shown in FIG. 14A , the mixed material is heated. The heating temperature is preferably 800°C or higher and 1100°C or lower, more preferably 900°C or higher and 1000°C or lower, and even more preferably about 950°C. If the temperature is too low, the decomposition and melting of the lithium source and the transition metal source may be insufficient. On the other hand, if the temperature is too high, defects may occur due to lithium evaporation from the lithium source and / or excessive reduction of the metal used as the transition metal source. For example, when cobalt is used as the transition metal, excessive reduction can cause cobalt to change from trivalent to divalent, which can induce oxygen defects.
[0260] The heating time is preferably from 1 hour to 100 hours, more preferably from 2 hours to 20 hours.
[0261] The temperature rise rate depends on the heating temperature reached, but is preferably 80° C. / h to 250° C. / h. For example, when heating at 1000° C. for 10 hours, the temperature rise rate should be 200° C. / h.
[0262] The heating atmosphere is preferably an atmosphere with little water, such as dry air, and for example, an atmosphere with a dew point of -50°C or less, more preferably an atmosphere with a dew point of -80°C or less. In this embodiment, heating is performed in an atmosphere with a dew point of -93°C. In addition, in order to suppress impurities that may be mixed into the material, the CH 4 , CO, CO 2 , and H 2 The impurity concentrations of the above should be 5 ppb (parts per billion) or less.
[0263] An oxygen-containing atmosphere is preferred as the heating atmosphere. For example, dry air can be continuously introduced into the reaction chamber. In this case, the flow rate of the dry air is preferably 10 L / min. The method of continuously introducing oxygen into the reaction chamber and allowing oxygen to flow through the reaction chamber is called flow.
[0264] When the heating atmosphere is an atmosphere containing oxygen, a method of not allowing oxygen to flow may be used. For example, a method of reducing the pressure of the reaction chamber and then filling it with oxygen to prevent the oxygen from entering or leaving the reaction chamber may be used, which is called purging. For example, the reaction chamber may be reduced in pressure to -970 hPa and then filled with oxygen to 50 hPa.
[0265] After heating, the material may be cooled naturally, but it is preferable that the time required for the temperature to drop from the specified temperature to room temperature is within a range of 10 to 50 hours. However, cooling to room temperature is not necessarily required, as long as the material is cooled to a temperature acceptable for the next step.
[0266] The heating in this step may be carried out using a rotary kiln or a roller hearth kiln. Heating in a rotary kiln can be carried out with stirring in either a continuous or batch system.
[0267] The crucible or sheath used during heating is preferably made of a highly heat-resistant material such as alumina (aluminum oxide), mullite / cordierite, magnesia, or zirconia. An alumina crucible is preferable because it is a material that does not contain impurities. In this embodiment, an alumina crucible with a purity of 99.9% is preferably used. It is preferable to heat the crucible or sheath with a lid, which prevents the material from volatilizing.
[0268] After heating, the material may be crushed and sieved as necessary. When recovering the heated material, it may be transferred from the crucible to a mortar and then recovered. It is preferable to use an alumina mortar. The alumina mortar is made of a material that does not contain impurities. Specifically, an alumina mortar with a purity of 90% or more, preferably 99% or more, is used. Heating conditions equivalent to those of step S13 can also be applied to heating steps other than step S13, which will be described later.
[0269] <Step S14> By the above steps, a composite oxide containing a transition metal (LiMO) is obtained in step S14 shown in FIG. 14A. 2 The composite oxide can be obtained as follows: 2It is sufficient for the lithium composite oxide to have a crystal structure represented by the formula: Li:M1:O = 1:1:2, and the composition is not strictly limited to Li:M1:O = 1:1:2. When cobalt is used as the transition metal, it is called a composite oxide containing cobalt and is represented by LiCoO2. The composition is not strictly limited to Li:Co:O = 1:1:2.
[0270] Although the example of producing the composite oxide by the solid phase method in steps S11 to S14 has been shown, the composite oxide may also be produced by a coprecipitation method or a hydrothermal method.
[0271] <Step S15> Next, in step S15 shown in Fig. 14A, the composite oxide is heated. Because this is the first heating of the composite oxide, the heating in step S15 may be referred to as initial heating. Alternatively, because this heating is performed before step S20 described below, it may be referred to as preheating or pretreatment.
[0272] The initial heating may cause lithium to be released from a portion of the lithium composite oxide in step S14. It is also expected to have the effect of increasing the crystallinity of the lithium composite oxide. Furthermore, since the lithium source and / or the transition metal M1 prepared in step S11 or the like contains impurities, the initial heating can reduce the amount of these impurities in the lithium composite oxide in step S14.
[0273] After the initial heating, the surface of the composite oxide becomes smooth. A smooth surface refers to a state in which there are few irregularities, the surface is rounded overall, and the corners are also rounded. Furthermore, a state in which there is little foreign matter adhering to the surface is called smooth. Foreign matter is thought to be a cause of irregularities, so it is preferable that no foreign matter adheres to the surface. A smooth active material can have a surface roughness of at least 10 nm or less, preferably less than 3 nm, when surface irregularity information is quantified from measurement data in a cross section observed with a scanning transmission electron microscope (STEM).
[0274] The initial heating is performed after the composite oxide is completed, and the initial heating is performed to smooth the surface, thereby reducing deterioration after charge and discharge. For the initial heating to smooth the surface, there is no need to prepare a lithium source.
[0275] Alternatively, in the initial heating step for smoothing the surface, it is not necessary to provide a source of the additive element.
[0276] Alternatively, in the initial heating step for smoothing the surface, no fluxing agent needs to be provided.
[0277] The lithium source and the transition metal source prepared in step S11 etc. may contain impurities. The initial heating can reduce the amount of impurities in the composite oxide completed in step S14.
[0278] The heating conditions for this step may be any conditions that result in a smooth surface of the composite oxide. For example, the heating conditions may be selected from those described in step S13. Regarding the heating conditions, the heating temperature for this step should be lower than the temperature for step S13 in order to maintain the crystalline structure of the composite oxide. Furthermore, the heating time for this step should be shorter than the time for step S13 in order to maintain the crystalline structure of the composite oxide. For example, heating at a temperature of 700°C or higher and 1000°C or lower for 2 hours or longer and 20 hours or shorter is recommended.
[0279] The heating in step S13 may cause a temperature difference between the surface and the interior of the composite oxide. The temperature difference may induce a contraction difference. It is also thought that the temperature difference causes a difference in fluidity between the surface and the interior, resulting in a contraction difference. The energy associated with the contraction difference causes a difference in internal stress in the composite oxide. The internal stress difference is also called strain, and this energy is sometimes called strain energy. The internal stress is removed by the initial heating in step S15; in other words, the strain energy is thought to be homogenized by the initial heating in step S15. When the strain energy is homogenized, the strain in the composite oxide is alleviated. Therefore, the surface of the composite oxide may become smoother after step S15. This is also called an improved surface. In other words, it is thought that the contraction difference that occurred in the composite oxide is alleviated after step S15, resulting in a smoother surface of the composite oxide.
[0280] Furthermore, the difference in shrinkage may cause microscopic deviations in the composite oxide, such as deviations in crystals. This step is preferably carried out in order to reduce such deviations. This step may potentially equalize the deviations in the composite oxide. Equalizing the deviations may result in a smoother surface of the composite oxide. This is also referred to as the alignment of crystal grains. In other words, it is believed that step S15 reduces deviations due to crystals or the like that have occurred in the composite oxide, resulting in a smoother surface of the composite oxide.
[0281] When a composite oxide with a smooth surface is used as a positive electrode active material, deterioration during charge and discharge in a secondary battery is reduced, and cracking of the positive electrode active material can be prevented.
[0282] The smooth surface of a composite oxide can be defined as a surface roughness of at least 10 nm or less, preferably less than 3 nm, when surface irregularity information is quantified from measurement data at a cross section of the composite oxide. The cross section is, for example, a cross section obtained when observing with a scanning transmission electron microscope (STEM).
[0283] Alternatively, a composite oxide containing lithium, a transition metal, and oxygen that has been synthesized in advance may be used in step S14. In this case, steps S11 to S13 can be omitted. By performing step S15 on a composite oxide that has been synthesized in advance, a composite oxide with a smooth surface can be obtained.
[0284] It is possible that the amount of lithium in the composite oxide is reduced by the initial heating. The lithium in the composite oxide may be more easily incorporated into the additive element, which will be explained in the next step S20.
[0285] <Step S20> The additive element X may be added to a composite oxide having a smooth surface, as long as it can form a layered rock salt crystal structure. Adding the additive element X to a composite oxide having a smooth surface allows the additive element X to be added evenly. Therefore, it is preferable to add the additive element X after the initial heating. The step of adding the additive element X will be described with reference to FIGS. 14B and 14C.
[0286] 14B, a Mg source and an F source are prepared as sources of additional elements (X sources) to be added to the composite oxide. A lithium source may also be prepared in addition to the additional element sources.
[0287] The additive element X can be one or more selected from nickel, cobalt, magnesium, calcium, chlorine, fluorine, aluminum, manganese, titanium, zirconium, yttrium, vanadium, iron, chromium, niobium, lanthanum, hafnium, zinc, silicon, sulfur, phosphorus, boron, and arsenic. The additive element X can also be one or more selected from bromine and beryllium. However, since bromine and beryllium are toxic to living organisms, it is more preferable to use the additive elements described above.
[0288] When magnesium is selected as the additional element X, the source of the additional element can be called a magnesium source. As the magnesium source, magnesium fluoride, magnesium oxide, magnesium hydroxide, magnesium carbonate, etc. may be used. Furthermore, a plurality of the above-mentioned magnesium sources may be used.
[0289] When fluorine is selected as the additive element X, the additive element source can be called a fluorine source. Examples of the fluorine source include lithium fluoride (LiF) and magnesium fluoride (MgF 2 ), aluminum fluoride (AlF 3 ), titanium fluoride (TiF 4 ), cobalt fluoride (CoF 2 , CoF 3 ), nickel fluoride (NiF 2 ), zirconium fluoride (ZrF 4 ), vanadium fluoride (VF 5 ), manganese fluoride, iron fluoride, chromium fluoride, niobium fluoride, zinc fluoride (ZnF 2 ), calcium fluoride (CaF 2 ), sodium fluoride (NaF), potassium fluoride (KF), barium fluoride (BaF 2 ), cerium fluoride (CeF 2 ), lanthanum fluoride (LaF 3 ), or sodium aluminum hexafluoride (Na 3 AlF 6 Among these, lithium fluoride is preferred because it has a relatively low melting point of 848° C. and is easily melted in the heating step described below.
[0290] Magnesium fluoride can be used as both a fluorine source and a magnesium source, and lithium fluoride can be used as a lithium source. Another lithium source that can be used in step S21 is lithium carbonate.
[0291] The fluorine source may also be gaseous, such as fluorine (F 2 ), fluorocarbon, sulfur fluoride, or oxygen fluoride (OF 2 , O 2 F 2 , O 3 F2 , O 4 F 2 , O 2 F) or the like may be used and mixed into the atmosphere in the heating step described below. Also, a plurality of the above-mentioned fluorine sources may be used.
[0292] In this embodiment, lithium fluoride (LiF) is prepared as the fluorine source, and magnesium fluoride (MgF) is prepared as the fluorine source and magnesium source. 2 Lithium fluoride and magnesium fluoride are prepared as LiF:MgF 2 Mixing them at a molar ratio of about LiF:MgF = 65:35 has the greatest effect of lowering the melting point (see Non-Patent Document 4). On the other hand, if the amount of lithium fluoride is too high, there is a concern that the lithium will be in excess and the cycle characteristics will deteriorate. Therefore, the molar ratio of lithium fluoride and magnesium fluoride is set to LiF:MgF 2 =x:1 (0≦x≦1.9), and LiF:MgF 2 =x:1 (0.1≦x≦0.5) is more preferable, and LiF:MgF 2 = x: 1 (x = near 0.33) is more preferable. Note that "near" refers to a value that is greater than 0.9 times and less than 1.1 times the value.
[0293] 14B, the magnesium source and the fluorine source are pulverized and mixed. This step can be performed under pulverization and mixing conditions selected from those described in step S12.
[0294] If necessary, a heating step may be performed after step S22. The heating step can be performed under heating conditions selected from those described in step S13. The heating time is preferably 2 hours or more, and the heating temperature is preferably 800°C or higher and 1100°C or lower.
[0295] 14B, the pulverized and mixed materials are collected to obtain an additive element source (X source). The additive element source shown in step S23 includes a plurality of starting materials and can be called a mixture.
[0296] The particle size of the mixture is preferably D50 (median diameter) of 600 nm to 20 μm, more preferably 1 μm to 10 μm. Even when a single material is used as the additive element source, the D50 (median diameter) is preferably 600 nm to 20 μm, more preferably 1 μm to 10 μm.
[0297] Such a finely powdered mixture (including the case where only one type of additive element is contained) makes it easier to uniformly adhere the mixture to the surface of the composite oxide particles when mixed with the composite oxide in a later step. Uniform adhesion of the mixture to the surface of the composite oxide is preferable because it makes it easier to uniformly distribute or diffuse the additive element in the surface layer portion of the composite oxide after heating. The region where the additive element is distributed can also be referred to as the surface layer portion. If there is a region in the surface layer that does not contain the additive element, it may be difficult to obtain the O3'-type crystal structure described below in the charged state. Although fluorine has been used in the explanation, fluorine may also be chlorine, and the term "halogen" can be used to refer to both.
[0298] <Step S21> A step different from that shown in Fig. 14B will be described with reference to Fig. 14C. In step S21 shown in Fig. 14C, four types of additive element sources to be added to the composite oxide are prepared. That is, the types of additive element sources in Fig. 14C are different from those in Fig. 14B. A lithium source may be prepared together with the additive element sources.
[0299] As sources of four additive elements, a magnesium source (Mg source), a fluorine source (F source), a nickel source (Ni source), and an aluminum source (Al source) are prepared. The magnesium source and the fluorine source can be selected from the compounds described with reference to FIG. 14B. Nickel oxide, nickel hydroxide, etc. can be used as the nickel source. Aluminum oxide, aluminum hydroxide, etc. can be used as the aluminum source.
[0300] <Steps S22 and S23> Next, steps S22 and S23 shown in FIG. 14C are the same as the steps described with reference to FIG. 14B.
[0301] 14A , the composite oxide and an additive element source (X source) are mixed. The ratio of the number of transition metal atoms M in the composite oxide containing lithium, transition metal, and oxygen to the number of magnesium atoms Mg in the additive element X is preferably M:Mg=100:y (0.1≦y≦6), and more preferably M:Mg=100:y (0.3≦y≦3).
[0302] The mixing conditions in step S31 are preferably milder than those in step S12 so as not to destroy the composite oxide. For example, it is preferable to use conditions with a lower rotation speed or shorter time than those in step S12. It can also be said that dry mixing provides milder conditions than wet mixing. For example, a ball mill, a bead mill, or the like can be used for mixing. When using a ball mill, it is preferable to use zirconia balls as the media.
[0303] In this embodiment, dry mixing is performed in a ball mill using zirconia balls with a diameter of 1 mm at 150 rpm for 1 hour in a dry room with a dew point of −100° C. or higher and −10° C. or lower.
[0304] <Step S32> Next, in step S32 of Fig. 14A, the mixed materials are collected to obtain a mixture 903. When collecting the materials, they may be crushed and then sieved, if necessary.
[0305] In this embodiment, a method is described in which lithium fluoride as a fluorine source and magnesium fluoride as a magnesium source are added to the composite oxide after the initial heating. However, the present invention is not limited to the above method. In step S11, that is, in the stage of the starting materials for the composite oxide, a magnesium source, a fluorine source, etc. can be added to the lithium source and the transition metal source. Then, in step S13, heating is performed to obtain LiMO to which magnesium and fluorine have been added. 2 In this case, it is not necessary to separate the steps S11 to S14 from the steps S21 to S23. This method is simple and has high productivity.
[0306] Alternatively, lithium cobalt oxide to which magnesium and fluorine have been added in advance may be used. If lithium cobalt oxide to which magnesium and fluorine have been added is used, steps S11 to S32 and step S20 can be omitted. This method can be said to be simple and highly productive.
[0307] Alternatively, a magnesium source and a fluorine source may be further added to lithium cobalt oxide to which magnesium and fluorine have been added in advance according to step S20 of FIG. 14B, or a magnesium source, a fluorine source, a nickel source, and an aluminum source may be further added according to step S20 of FIG. 14C.
[0308] 14A, the mixture 903 is heated. The heating can be performed under the heating conditions selected from those described in step S13. The heating time is preferably 2 hours or more.
[0309] Here, a supplementary note about the heating temperature will be given. The lower limit of the heating temperature in step S33 is 2 The temperature at which the reaction between LiMO and the additive element source proceeds must be equal to or higher than the temperature at which the reaction between LiMO and the additive element source proceeds. 2 The temperature may be lower than the melting point of these materials as long as it is a temperature at which mutual diffusion of elements contained in the oxide and the additive element source occurs. m 0.757 times (Tammann temperature T d ) solid-phase diffusion occurs. Therefore, the heating temperature in step S33 should be 500° C. or higher.
[0310] Of course, the reaction proceeds more easily when the temperature is equal to or higher than the temperature at which at least a part of the mixture 903 melts. 2 When LiF and MgF 2 The eutectic point of the alloy is around 742° C. Therefore, it is preferable that the lower limit of the heating temperature in step S33 is 742° C. or higher.
[0311] Also, LiCoO 2 :LiF:MgF 2A mixture 903 obtained by mixing the components so that the molar ratio was 100:0.33:1 exhibits an endothermic peak at around 830° C. in differential scanning calorimetry (DSC). Therefore, the lower limit of the heating temperature is more preferably 830° C. or higher.
[0312] A higher heating temperature is preferable because the reaction proceeds more easily, the heating time is shorter, and productivity is higher.
[0313] The upper limit of the heating temperature is LiMO 2 Decomposition temperature of LiCoO 2 The decomposition temperature of LiM1O is less than 1130°C. At temperatures close to the decomposition temperature, a small amount of LiM1O 2 Therefore, the temperature is more preferably 1000°C or lower, even more preferably 950°C or lower, and even more preferably 900°C or lower.
[0314] Taking these factors into consideration, the heating temperature in step S33 is preferably 500°C or higher and 1130°C or lower, more preferably 500°C or higher and 1000°C or lower, even more preferably 500°C or higher and 950°C or lower, and even more preferably 500°C or higher and 900°C or lower. Also, it is preferably 742°C or higher and 1130°C or lower, more preferably 742°C or higher and 1000°C or lower, even more preferably 742°C or higher and 950°C or lower, and even more preferably 742°C or higher and 900°C or lower. Also, it is preferably 800°C or higher and 1100°C or lower, or 830°C or higher and 1130°C or lower, more preferably 830°C or higher and 1000°C or lower, even more preferably 830°C or higher and 950°C or lower, and even more preferably 830°C or higher and 900°C or lower. The heating temperature in step S33 is preferably higher than that in step S13.
[0315] Furthermore, when the mixture 903 is heated, it is preferable to control the partial pressure of fluorine or fluoride resulting from the fluorine source or the like within an appropriate range.
[0316] In the manufacturing method described in this embodiment, some materials, for example, LiF, which is a fluorine source, may function as a flux. This function allows the heating temperature to be controlled by the composite oxide (LiMO). 2) can be heated to a temperature lower than the decomposition temperature, for example, 742°C to 950°C, and additive elements such as magnesium can be distributed in the surface layer, thereby producing a positive electrode active material with good characteristics.
[0317] However, since LiF has a lower specific gravity in a gaseous state than oxygen, there is a possibility that LiF will volatilize when heated, and if it volatilizes, the amount of LiF in the mixture 903 will decrease. This will weaken its function as a flux. Therefore, it is necessary to heat while suppressing the volatilization of LiF. Even if LiF is not used as a fluorine source, etc., LiM1O 2 There is a possibility that Li on the surface reacts with F in the fluorine source to produce LiF, which may then volatilize. Therefore, even if a fluoride with a higher melting point than LiF is used, it is still necessary to suppress volatilization.
[0318] Therefore, it is preferable to heat the mixture 903 in an atmosphere containing LiF, that is, to heat the mixture 903 in a state where the partial pressure of LiF is high in the heating furnace. By heating in this manner, it is possible to suppress the volatilization of LiF in the mixture 903.
[0319] The heating in this step is preferably performed so as not to cause adhesion of particles of the mixture 903. If the particles of the mixture 903 adhere to each other during heating, the contact area with oxygen in the atmosphere decreases, and the route along which the additive elements (e.g., fluorine) diffuse is blocked, which may result in poor distribution of the additive elements (e.g., magnesium and fluorine) in the surface layer portion.
[0320] It is also believed that uniform distribution of the additive element (e.g., fluorine) in the surface layer results in a smooth, less uneven cathode active material. Therefore, in order to maintain or further smooth the surface after heating in step S15 in this process, it is better for the particles not to adhere to each other.
[0321] Furthermore, when heating in a rotary kiln, it is preferable to control the flow rate of the oxygen-containing atmosphere in the kiln during heating. For example, it is preferable to reduce the flow rate of the oxygen-containing atmosphere, or to first purge the atmosphere and then not flow the atmosphere after introducing the oxygen atmosphere into the kiln. Flowing oxygen may cause the fluorine source to evaporate, which is undesirable in terms of maintaining surface smoothness.
[0322] When heating is performed using a roller hearth kiln, the mixture 903 can be heated in an atmosphere containing LiF by, for example, placing a lid on a container containing the mixture 903 .
[0323] The heating time is determined by the heating temperature, the amount of LiM1O in step S14, 2 It varies depending on the particle size and composition of LiMO. 2 If the size of is small, LiMO 2 A lower temperature or shorter time may be more preferable than when the magnitude of
[0324] The composite oxide (LiMO) in step S14 of FIG. 2 When the median diameter (D50) of the powder is about 12 μm, the heating temperature is preferably, for example, 600° C. or higher and 950° C. or lower. The heating time is, for example, preferably 3 hours or higher, more preferably 10 hours or higher, and even more preferably 60 hours or higher. The cooling time after heating is preferably, for example, 10 hours or higher and 50 hours or lower.
[0325] On the other hand, the composite oxide (LiMO) of step S14 2 When the median diameter (D50) of the powder is about 5 μm, the heating temperature is preferably, for example, 600° C. or higher and 950° C. or lower. The heating time is preferably, for example, 1 hour or higher and 10 hours or lower, and more preferably about 2 hours. The cooling time after heating is preferably, for example, 10 hours or higher and 50 hours or lower.
[0326] <Step S34> Next, in step S34 shown in FIG. 14A , the heated material is recovered and crushed as necessary to obtain a positive electrode active material 100E. At this time, it is preferable to further sieve the recovered particles. Through the above steps, a positive electrode active material 100E according to one embodiment of the present invention can be produced. The positive electrode active material according to one embodiment of the present invention has a smooth surface. The positive electrode active material 100E can be used as the first material 100x shown in Embodiments 1 and 2.
[0327] [Method 5 for Producing Positive Electrode Active Material] Next, a method for carrying out the present invention, which is different from Method 2 for Producing Positive Electrode Active Material, will be described.
[0328] In FIG. 15, steps S11 to S15 are performed in the same manner as in FIG. 14A to obtain a composite oxide (LiMO) with a smooth surface. 2 ) to prepare.
[0329] <Step S20a> As described above, the additive element X may be added to the composite oxide within a range that allows a layered rock-salt type crystal structure to be formed. In this production method 2, however, a step of adding the additive element in two or more batches will be described with reference to FIG. 16A as well.
[0330] <Step S21> Figure 16A shows the details of step S20a. In step S21, a Mg source and an F source are prepared as the first additive element source (X1 source). The X1 source can be selected from the additive elements X described in step S21 shown in Figure 14B and used. For example, one or more selected from magnesium, fluorine, and calcium can be suitably used as the additive element X1. Figure 16A illustrates an example in which a magnesium source (Mg source) and a fluorine source (F source) are used as the first additive element source (X1 source).
[0331] Steps S21 to S23 shown in Fig. 16A can be fabricated under the same conditions as steps S21 to S23 shown in Fig. 14B. As a result, a first additive element source (X1 source) can be obtained in step S23. The first additive element source (X1 source) is the X1 source of step S20a shown in Fig. 15.
[0332] Steps S31 to S33 shown in FIG. 15 can be fabricated in the same manner as steps S31 to S33 shown in FIG. 14A.
[0333] <Step S34a> Next, the material heated in step S33 shown in Fig. 15 is recovered to prepare a composite oxide containing the additional element X1. This is also called a second composite oxide to distinguish it from the composite oxide in step S14.
[0334] <Step S40> In step S40 shown in Fig. 15, a second additive element source (X2 source) is added. Details of step S40 will be described with reference to Figs. 16B and 16C.
[0335] <Step S41> In step S41 shown in FIG. 16B, a Ni source and an Al source are prepared as a second additive element source (X2 source). The X2 source can be selected from the additive elements X described in step S21 shown in FIG. 14B. For example, the additive element X2 can be any one or more selected from nickel, titanium, boron, zirconium, and aluminum. FIG. 16B illustrates an example in which a nickel source and an aluminum source are used as the second additive element source (X2 source).
[0336] Steps S41 to S43 shown in Fig. 16B can be fabricated under the same conditions as steps S21 to S23 shown in Fig. 14B. As a result, the second additive element source (X2 source) can be obtained in step S43.
[0337] 16C shows a modified example of the steps described with reference to FIG. 16B. In step S41 shown in FIG. 16C, a nickel source (Ni source) and an aluminum source (Al source) are prepared, and in step S42a, they are independently pulverized. As a result, in step S43, a plurality of second additive element sources (X2 sources) are prepared. The steps of FIG. 16C differ from those of FIG. 16B in that the additive elements are independently pulverized in step S42a.
[0338] <Steps S51 to S53> Next, steps S51 to S53 shown in FIG. 15 can be performed under the same conditions as steps S31 to S33 shown in FIG. 14A. The heating step in step S53 can be performed at a lower temperature and for a shorter time than in step S33. Through the above steps, step S53 can produce a positive electrode active material 100F according to one embodiment of the present invention. The positive electrode active material according to one embodiment of the present invention has a smooth surface. The positive electrode active material 100F can be used as the first material 100x described in Embodiments 1 and 2.
[0339] 15 and 16 , in the preparation method 2, the additive element to the composite oxide is introduced separately as a first additive element X1 and a second additive element X2. By introducing the additive elements separately, the depth profile of each additive element can be changed. For example, it is possible to profile the first additive element so that its concentration is higher in the surface layer portion than in the interior, and profile the second additive element so that its concentration is higher in the interior than in the surface layer portion.
[0340] After the initial heating described in this embodiment, a positive electrode active material with a smooth surface can be obtained.
[0341] The initial heating shown in this embodiment is performed on the composite oxide. Therefore, the initial heating is preferably performed under conditions that are lower than the heating temperature for obtaining the composite oxide and shorter than the heating time for obtaining the composite oxide. When an additional element is added to the composite oxide, it is preferable to perform the addition step after the initial heating. The addition step can be divided into two or more steps. Following this step order is preferable because the surface smoothness obtained by the initial heating is maintained. When the composite oxide contains cobalt as a transition metal, it can be interpreted as a composite oxide containing cobalt.
[0342] The positive electrode active material 100F is a composite oxide containing lithium, a transition metal, and oxygen (LiMO 2 However, the positive electrode active material of one embodiment of the present invention may be expressed as LiMO 2The composition is not strictly limited to Li:M1:O=1:1:2, so long as it has a crystalline structure of a lithium composite oxide represented by the formula:
[0343] As described above, in one aspect of the present invention, a cathode active material is prepared using a high-purity transition metal source during synthesis, and the synthesis process involves minimal impurity contamination. The cathode active material obtained by this method for preparing a cathode active material has a low impurity concentration, in other words, is a highly purified material. Furthermore, the cathode active material obtained by this method for preparing a cathode active material is a material with high crystallinity. Furthermore, the cathode active material obtained by the method for preparing a cathode active material of one aspect of the present invention can increase the capacity of a secondary battery and / or improve the reliability of the secondary battery.
[0344] [Structure of Positive Electrode Active Material] Positive electrode active materials of embodiments of the present invention will be described with reference to FIGS.
[0345] 17A is a schematic top view of a positive electrode active material 100 according to one embodiment of the present invention. FIG. 17B is a schematic cross-sectional view taken along line A-B in FIG. 17A.
[0346] <Contained Elements and Distribution> The positive electrode active material 100 contains lithium, a transition metal, oxygen, and an additive element. The additive element may be an element different from the transition metal contained in the positive electrode active material 100. That is, the positive electrode active material 100 contains LiMO 2 It can be said that the compound oxide represented by the formula (I) is added with elements other than M1.
[0347] The transition metal contained in the positive electrode active material 100 is preferably a metal capable of forming a layered rock-salt composite oxide belonging to the space group R-3m with lithium. For example, at least one of manganese, cobalt, and nickel can be used. That is, the transition metal contained in the positive electrode active material 100 may be cobalt alone, nickel alone, a combination of cobalt and manganese, or a combination of cobalt and nickel, or three of cobalt, manganese, and nickel. That is, the positive electrode active material 100 may contain a composite oxide containing lithium and a transition metal, such as lithium cobalt oxide, lithium nickel oxide, lithium cobalt oxide in which some of the cobalt is replaced with manganese, lithium cobalt oxide in which some of the cobalt is replaced with nickel, or nickel-manganese-lithium cobalt oxide. Including nickel in addition to cobalt as a transition metal is preferable because the crystal structure becomes more stable during charging at high voltages.
[0348] The additive element X contained in the positive electrode active material 100 is preferably one or more selected from nickel, cobalt, magnesium, calcium, chlorine, fluorine, aluminum, manganese, titanium, zirconium, yttrium, vanadium, iron, chromium, niobium, lanthanum, hafnium, zinc, silicon, sulfur, phosphorus, boron, and arsenic. These additive elements may further stabilize the crystalline structure of the positive electrode active material 100. That is, the positive electrode active material 100 may include lithium cobalt oxide doped with magnesium and fluorine, lithium cobalt oxide doped with magnesium, fluorine, and titanium, lithium nickel-cobalt oxide doped with magnesium and fluorine, lithium cobalt-aluminate doped with magnesium and fluorine, nickel-cobalt-aluminate doped with magnesium and fluorine, nickel-manganese-cobalt oxide doped with magnesium and fluorine, and the like. In this specification and the like, the additive element X may be referred to interchangeably as a mixture, a part of a raw material, or the like.
[0349] As shown in FIG. 17B , the positive electrode active material 100 has a surface layer 100a and an interior 100b. The surface layer 100a preferably has a higher concentration of the additive element than the interior 100b. Furthermore, as shown by the gradation in FIG. 17B , the additive element preferably has a concentration gradient that increases from the interior toward the surface. In this specification and the like, the surface layer 100a refers to the region extending from the surface of the positive electrode active material 100 to a depth of approximately 10 nm. Surfaces resulting from cracks and / or fissures may also be considered the surface. Furthermore, the region deeper than the surface layer 100a of the positive electrode active material 100 is referred to as the interior 100b.
[0350] In the positive electrode active material 100 of one embodiment of the present invention, even if lithium is released from the positive electrode active material 100 upon charging, the surface layer portion 100a, i.e., the outer periphery of the particle, having a high concentration of the added element, reinforces the layered structure consisting of octahedra of cobalt and oxygen so as not to be destroyed.
[0351] Furthermore, the concentration gradient of the additive element is preferably present throughout the entire surface layer 100a of the positive electrode active material 100, and more preferably uniformly. This is because even if a portion of the surface layer 100a is reinforced, if there is a portion without reinforcement, stress may be concentrated in the unreinforced portion, which is undesirable. If stress is concentrated in a portion of the particle, defects such as cracks may occur there, which may lead to breakage of the positive electrode active material and a decrease in charge / discharge capacity.
[0352] Magnesium is divalent and is more stable at the lithium site than at the transition metal site in the layered rock-salt crystal structure, and therefore more likely to enter the lithium site. The presence of magnesium at an appropriate concentration at the lithium site in the surface layer 100a facilitates the maintenance of the layered rock-salt crystal structure. Furthermore, magnesium has a strong bond with oxygen, which can inhibit the desorption of oxygen around magnesium. At an appropriate concentration, magnesium is preferable because it does not adversely affect the intercalation and deintercalation of lithium during charge and discharge. However, excessive magnesium may adversely affect the intercalation and deintercalation of lithium.
[0353] Aluminum is trivalent and can exist at the transition metal site in the layered rock salt crystal structure. Aluminum can suppress the elution of surrounding cobalt. Furthermore, because aluminum has a strong bond with oxygen, it can suppress the release of oxygen from the surrounding area of aluminum. Therefore, the addition of aluminum as an additive element can result in a positive electrode active material 100 whose crystal structure is less likely to collapse even after repeated charge and discharge.
[0354] Fluorine is a monovalent anion, and when part of the oxygen in the surface layer portion 100a is substituted with fluorine, the lithium desorption energy is reduced. This is because the valence of cobalt ions changes with lithium desorption, from trivalent to tetravalent in the absence of fluorine, and from divalent to trivalent in the presence of fluorine, resulting in different oxidation-reduction potentials. Therefore, when part of the oxygen in the surface layer portion 100a of the positive electrode active material 100 is substituted with fluorine, it can be said that desorption and insertion of lithium ions near the fluorine is more likely to occur smoothly. Therefore, when used in a secondary battery, charge / discharge characteristics, rate characteristics, etc. are improved, which is preferable.
[0355] Titanium oxide is known to have superhydrophilic properties. Therefore, by forming the cathode active material 100 with titanium oxide in the surface layer portion 100a, it is possible that the cathode active material 100 has good wettability with highly polar solvents. When formed into a secondary battery, it is possible that the interface between the cathode active material 100 and a highly polar electrolyte solution will have good contact, thereby suppressing an increase in resistance. In this specification and the like, the electrolyte solution corresponds to a liquid electrolyte.
[0356] As the charging voltage of a secondary battery increases, the voltage of the positive electrode generally increases. The positive electrode active material of one embodiment of the present invention has a stable crystal structure even at high voltages. The stable crystal structure of the positive electrode active material in a charged state can suppress a decrease in capacity due to repeated charge and discharge.
[0357] Furthermore, a short circuit in a secondary battery not only causes problems in the charging and / or discharging operations of the secondary battery, but may also lead to heat generation and fire. To achieve a safe secondary battery, it is preferable that a short circuit current be suppressed even at a high charging voltage. The positive electrode active material 100 of one embodiment of the present invention suppresses a short circuit current even at a high charging voltage. Therefore, a secondary battery that achieves both high capacity and safety can be obtained.
[0358] A secondary battery using the positive electrode active material 100 of one embodiment of the present invention preferably simultaneously satisfies high capacity, excellent charge / discharge cycle characteristics, and safety.
[0359] The concentration gradient of the added element can be evaluated, for example, using energy dispersive X-ray spectroscopy (EDX). Among EDX measurements, measuring while scanning an area and evaluating the area two-dimensionally is sometimes called EDX area analysis. Furthermore, extracting data of a linear area from EDX area analysis and evaluating the distribution of atomic concentration in the positive electrode active material is sometimes called line analysis.
[0360] EDX area analysis (e.g., element mapping) can quantitatively analyze the concentration of the added element in the surface layer portion 100a, the interior portion 100b, and the vicinity of the grain boundaries of the positive electrode active material 100. Furthermore, EDX ray analysis can analyze the concentration peak of the added element.
[0361] When EDX-ray analysis is performed on the positive electrode active material 100, the peak of the magnesium concentration in the surface layer portion 100a is preferably present at a depth of up to 3 nm from the surface of the positive electrode active material 100 toward the center, more preferably at a depth of up to 1 nm, and even more preferably at a depth of up to 0.5 nm.
[0362] Furthermore, the fluorine distribution in the positive electrode active material 100 preferably overlaps with the magnesium distribution, and therefore, when EDX-ray analysis is performed, the peak of the fluorine concentration in the surface layer portion 100 a preferably exists within a depth of 3 nm from the surface of the positive electrode active material 100 toward the center, more preferably within a depth of 1 nm, and even more preferably within a depth of 0.5 nm.
[0363] It is not necessary for all additive elements to have the same concentration distribution. For example, when the positive electrode active material 100 contains aluminum as an additive element, it is preferable that the distribution be slightly different from that of magnesium and fluorine. For example, when EDX-ray analysis is performed, it is preferable that the magnesium concentration peak is closer to the surface than the aluminum concentration peak in the surface layer portion 100a. For example, the aluminum concentration peak is preferably present at a depth of 0.5 nm to 20 nm from the surface toward the center of the positive electrode active material 100, and more preferably at a depth of 1 nm to 5 nm.
[0364] Furthermore, when the positive electrode active material 100 is subjected to linear or area analysis, the ratio of the additive element I to the transition metal (I / M) near the grain boundaries is preferably 0.020 or more and 0.50 or less. It is even more preferably 0.025 or more and 0.30 or less. It is even more preferably 0.030 or more and 0.20 or less. For example, when the additive element is magnesium and the transition metal is cobalt, the ratio of the number of magnesium atoms to the number of cobalt atoms (Mg / Co) is preferably 0.020 or more and 0.50 or less. It is even more preferably 0.025 or more and 0.30 or less. It is even more preferably 0.030 or more and 0.20 or less.
[0365] As mentioned above, if the additive element contained in the positive electrode active material 100 is excessive, it may adversely affect the insertion and extraction of lithium. Furthermore, when used as a secondary battery, it may also result in an increase in resistance and a decrease in capacity. On the other hand, if the additive element is insufficient, it may not be distributed throughout the entire surface layer portion 100a, and the effect of maintaining the crystalline structure may be insufficient. Thus, the additive element needs to be present at an appropriate concentration in the positive electrode active material 100, but adjusting this concentration is not easy.
[0366] Therefore, for example, the positive electrode active material 100 may have a region where an excess of the additive element is unevenly distributed. The presence of such a region allows the excess additive element to be removed from other regions, thereby achieving an appropriate additive element concentration in the interior of the positive electrode active material 100 and in most of the vicinity of the surface. By achieving an appropriate additive element concentration in the interior of the positive electrode active material 100 and in most of the vicinity of the surface, an increase in resistance and a decrease in capacity when the positive electrode active material 100 is used as a secondary battery can be suppressed. The ability to suppress an increase in resistance of a secondary battery is an extremely desirable characteristic, particularly during high-rate charging and discharging.
[0367] Furthermore, in the positive electrode active material 100 having a region where the excess additive element is unevenly distributed, it is permissible to mix the additive element in excess to some extent in the manufacturing process, which is preferable because it widens the margin in production.
[0368] In this specification and the like, uneven distribution refers to the difference in the concentration of a certain element between a certain region A and a certain region B. It may also be referred to as segregation, precipitation, non-uniformity, deviation, high concentration or low concentration, etc.
[0369] <Crystal structure> Lithium cobalt oxide (LiCoO 2 Materials having a layered rock salt type crystal structure, such as LiM1O2, have a high discharge capacity and are known to be excellent as positive electrode active materials for secondary batteries. 2 Examples of the composite oxide include those represented by the following formula:
[0370] It is known that the strength of the Jahn-Teller effect in transition metal compounds varies depending on the number of electrons in the d orbital of the transition metal.
[0371] In composite oxides containing nickel, distortion may easily occur due to the Jahn-Teller effect. 2 When LiCoO is charged and discharged at a high voltage, there is a concern that the crystal structure may be destroyed due to distortion. 2 It is suggested that the influence of the Jahn-Teller effect is small in this case, and the durability of charge and discharge at high voltages may be superior, which is preferable.
[0372] The positive electrode active material will be described with reference to Fig. 18 to Fig. 21. Fig. 18 to Fig. 21 describe a case where cobalt is used as the transition metal contained in the positive electrode active material.
[0373] <Li x CoO 2 When x is 1 in the positive electrode active material 100 of one embodiment of the present invention is in a discharged state, that is, Li x CoO 2 In the case where x = 1 in the formula (I), it is preferable that the composite oxide has a layered rock-salt type crystal structure belonging to the space group R-3m. The layered rock-salt type composite oxide has a high discharge capacity, has two-dimensional lithium ion diffusion paths, is suitable for lithium ion insertion / extraction reactions, and is excellent as a positive electrode active material for secondary batteries. Therefore, it is particularly preferable that the inner portion 100b, which occupies the majority of the volume of the positive electrode active material 100, has a layered rock-salt type crystal structure.
[0374] In Figure 18, the layered rock salt crystal structure is added to the space group R-3m and O3 is added. The name O3 comes from the fact that in this crystal structure, lithium occupies an octahedral site and CoO 2 This name is based on the existence of three layers. This crystal structure is also sometimes called an O3 type crystal structure. 2 The layer is an octahedral structure in which cobalt is six-coordinated with oxygen, and the structure is continuous in the plane direction with edge sharing. 2 The layer is sometimes referred to as a layer of cobalt and oxygen octahedra.
[0375] <Li x CoO 2 State in which x is small in the positive electrode active material 100 of one embodiment of the present invention x CoO 2 The crystal structure when x is small differs from that of conventional positive electrode active materials. Here, "small x" means 0.1<x≦0.24. Figure 18 shows the crystal structure when x = 0.2.
[0376] Li x CoO 2 A conventional positive electrode active material and the positive electrode active material 100 of one embodiment of the present invention are compared with each other in terms of changes in the crystal structure that occur with changes in x in the positive electrode active material.
[0377] <Conventional Positive Electrode Active Material> The change in the crystal structure of a conventional positive electrode active material is shown in FIG. 20. The conventional positive electrode active material shown in FIG. 20 is lithium cobalt oxide (LiCoO 2 , LCO). As described in Non-Patent Documents 1 to 3, the crystal structure of the lithium cobalt oxide shown in FIG.
[0378] In Figure 20, x CoO 2 The crystal structure of lithium cobalt oxide with x = 1 is shown with R-3m O3 attached. x = 1 corresponds to the discharged state of the secondary battery. Next, the crystal structure of lithium cobalt oxide with x = 0.5 is shown with P2 / m monoclinic O1 attached. Conventional lithium cobalt oxide has a crystal structure that belongs to the monoclinic space group P2 / m when the symmetry of lithium increases at around x = 0.5. This structure has CoO in the unit cell. 2 There is one layer. Therefore, this crystal structure is sometimes called O1 type or monoclinic O1 type.
[0379] Also Li x CoO 2 The crystal structure of lithium cobalt oxide when x = 0 is shown in the figure, along with P-3m1 trigonal O1. Conventional lithium cobalt oxide has a crystal structure that belongs to the trigonal space group P-3m1 when x = 0. This structure has CoO in the unit cell. 2 There is one layer. Therefore, this crystal structure is sometimes called O1 type or trigonal O1 type. In addition, when the trigonal crystal is converted into a composite hexagonal lattice, this crystal structure is sometimes called hexagonal O1 type.
[0380] Also Li x CoO 2 The crystal structure of lithium cobalt oxide when x = 0.12 is shown with R-3m H1-3 attached. Conventional lithium cobalt oxide has a crystal structure that belongs to the space group R-3m when x = 0.12. This structure is similar to CoO, such as trigonal O1 type. 2 and LiCoO such as R-3m O 2It can also be said that the structure of and are stacked alternately. Therefore, this crystal structure is sometimes referred to as the H1-3 type crystal structure. Note that, since actual lithium insertion and extraction can be uneven, the H1-3 type crystal structure is experimentally observed from about x = 0.25. In addition, the number of cobalt atoms per unit cell in the H1-3 type crystal structure is actually twice that of other structures. However, in Figure 20 and other parts of this specification, the c-axis of the H1-3 type crystal structure is shown as 1 / 2 of the unit cell to facilitate comparison with other crystal structures.
[0381] As an example of the H1-3 type crystal structure, as described in Non-Patent Document 2, the coordinates of cobalt and oxygen in the unit cell can be expressed as Co (0, 0, 0.42150 ± 0.00016), O1 (0, 0, 0.27671 ± 0.00045), and O2 (0, 0, 0.11535 ± 0.00045). O1 and O2 are each oxygen atoms. Which unit cell should be used to represent the crystal structure of the positive electrode active material can be determined, for example, by Rietveld analysis of XRD. In this case, it is sufficient to adopt a unit cell that results in a small GOF (goodness of fit) value.
[0382] Li x CoO 2 When charging and discharging are repeated so that x in the formula is 0.24 or less, conventional lithium cobalt oxide undergoes repeated changes in crystal structure (i.e., non-equilibrium phase changes) between the H1-3 type crystal structure and the R-3m O3 structure in the discharged state.
[0383] However, these two crystal structures are different from CoO 2 As shown by the dotted lines and arrows in FIG. 20, in the H1-3 type crystal structure, CoO 2 The layers are significantly deviated from R-3m O3. Such dynamic structural changes can adversely affect the stability of the crystal structure.
[0384] Furthermore, the difference in volume between these two crystal structures is large: per the same number of cobalt atoms, the difference in volume between the H1-3 crystal structure and the discharged R-3mO3 crystal structure is greater than 3.5%, typically 3.9% or more.
[0385] In addition, the H1-3 type crystal structure has CoO like the trigonal O1 type. 2 There is no lithium between the layers, and CoO 2 A structure with continuous layers is likely to be unstable.
[0386] Therefore, when charging and discharging is repeated so that x becomes 0.24 or less, the crystal structure of conventional lithium cobalt oxide collapses. This collapse of the crystal structure causes a deterioration in cycle characteristics. This is because the collapse of the crystal structure reduces the number of sites where lithium can exist stably and makes it difficult for lithium to be inserted and extracted.
[0387] <Positive Electrode Active Material of One Embodiment of the Present Invention> In the positive electrode active material 100 of one embodiment of the present invention shown in FIG. x CoO 2 The change in the crystal structure between the discharge state where x is 1 and the state where x is 0.24 or less, for example, x = 0.2, is smaller than that of conventional positive electrode active materials. More specifically, the change in the crystal structure between the discharge state where x is 1 and the state where x is 0.2, i.e., 0.2, is smaller than that of conventional positive electrode active materials. 2 The layer misalignment can be reduced. Furthermore, the change in volume per cobalt atom can be reduced. Therefore, the positive electrode active material 100 of one embodiment of the present invention is less likely to lose its crystal structure even when repeatedly charged and discharged so that x is 0.24 or less, and excellent cycle characteristics can be achieved.
[0388] The positive electrode active material 100 according to one embodiment of the present invention is Li x CoO 2 When x is 0.24 or less, the positive electrode active material 100 can have a more stable crystal structure than conventional positive electrode active materials. x CoO 2 When the value of x is kept at 0.24 or less, short circuits are less likely to occur and the safety of the secondary battery is further improved, which is preferable.
[0389] Li x CoO 2The crystal structure of lithium cobalt oxide when x is approximately 1 or 0.2 is shown in Figure 18. It is a composite oxide containing lithium cobalt oxide, cobalt as a transition metal, and oxygen. In addition to the above, it preferably contains magnesium as an additive element. It is also preferably contains a halogen such as fluorine or chlorine as an additive element.
[0390] The lithium cobalt oxide of one embodiment of the present invention has the same R-3m O3 crystal structure as conventional lithium cobalt oxide when x = 1. The lithium cobalt oxide of one embodiment of the present invention has a crystal structure different from conventional lithium cobalt oxide when x is 0.24 or less, for example, about 0.2, at which point conventional lithium cobalt oxide has an H1-3 type crystal structure.
[0391] When x is about 0.2, the lithium cobalt oxide of one embodiment of the present invention has a crystal structure belonging to the trigonal space group R-3m. 2 The symmetry of the layers is the same as that of O3. Therefore, this crystal structure is called an O3'-type crystal structure. In addition, in Figure 18, R-3m O3' is added to the crystal structure when x = 0.2.
[0392] The O3' type crystal structure can show the coordinates of cobalt and oxygen in the unit cell as Co(0,0,0.5), O(0,0,x), with 0.20≦x≦0.25.
[0393] As shown by the dotted line in FIG. 18, the R-3m O3 in the discharged state and the O3′-type crystal structure are different from CoO 2 There is almost no layer misalignment.
[0394] The difference in volume per the same number of cobalt atoms between R-3m O3 in a discharged state and the O3' type crystal structure is 2.5% or less, more specifically 2.2% or less, typically 1.8%, which is a small volume difference.
[0395] In this way, in the positive electrode active material 100, Li x CoO 2When x is small, i.e., when a large amount of lithium is released, the change in crystal structure is suppressed compared to conventional positive electrode active materials. Furthermore, the change in volume is also suppressed when compared per the same number of cobalt atoms. Therefore, the positive electrode active material 100 is resistant to collapse of its crystal structure even when repeatedly charged and discharged so that x is 0.24 or less. Therefore, the decrease in charge / discharge capacity during charge / discharge cycles is suppressed. Furthermore, because more lithium can be stably utilized than in conventional positive electrode active materials, the positive electrode active material 100 has a large discharge capacity per weight and per volume. Therefore, by using the positive electrode active material 100, a secondary battery with a high discharge capacity per weight and per volume can be fabricated.
[0396] The positive electrode active material 100 is Li x CoO 2 It has been confirmed that when x is 0.15 or more and 0.24 or less, it may have an O3' type crystal structure, and it is presumed that it also has an O3' type crystal structure when x is more than 0.24 and 0.27 or less. However, the crystal structure is x CoO 2 Since the influence is due to factors such as the number of charge / discharge cycles, charge / discharge current, temperature, electrolyte, etc., as well as the value of x in the formula (I), the O3'-type crystal structure may be obtained regardless of the above range of x.
[0397] The positive electrode active material 100 is Li x CoO 2 When x is greater than 0.1 and equal to or less than 0.24, the entire interior of the positive electrode active material 100 does not have to have the O3′-type crystal structure, but may contain other crystal structures, or may be partially amorphous.
[0398] Also Li x CoO 2 To make the value of x small, it is generally necessary to charge at a high charging voltage. x CoO 2In other words, a state in which x is small can be said to be a state in which the battery is charged at a high charging voltage. For example, when a conventional positive electrode active material is charged at a voltage of 4.6 V or higher relative to the potential of lithium metal in an environment of 25°C, an H1-3 crystal structure appears. Therefore, a high charging voltage relative to the potential of lithium metal can be said to be a charging voltage of 4.6 V or higher. Furthermore, in this specification and the like, unless otherwise specified, the charging voltage will be expressed relative to the potential of lithium metal.
[0399] Charging the positive electrode active material 100 at a high charging voltage is preferable because it can maintain the symmetrical crystal structure of R-3mO. An example of a high charging voltage is a voltage of 4.6 V or more at 25° C. Another example of a higher charging voltage is a voltage of 4.65 V or more and 4.7 V or less at 25° C.
[0400] When the charge voltage is further increased, H1-3 type crystals may be gradually observed even in the positive electrode active material 100. As described above, the crystal structure is affected by the number of charge / discharge cycles, the charge / discharge current, the electrolyte, and the like. Therefore, when the charge voltage is lower, for example, even when the charge voltage is 4.5 V or higher but lower than 4.6 V at 25° C., the positive electrode active material 100 of one embodiment of the present invention may be able to adopt an O3′ type crystal structure.
[0401] In addition, when graphite is used as the negative electrode active material in a secondary battery, the voltage of the secondary battery is lower than the above by the potential of the graphite. The potential of graphite is about 0.05 V to 0.2 V with respect to the potential of lithium metal. Therefore, in the case of a secondary battery using graphite as the negative electrode active material, the same crystal structure is maintained at a voltage obtained by subtracting the potential of graphite from the above voltage.
[0402] In addition, in O3' of FIG. 18, lithium is shown to exist at all lithium sites with equal probability, but this is not limited to this. It may exist unevenly at some lithium sites, or, for example, in the monoclinic O1 (Li 0.5 CoO 2 The distribution of lithium can be analyzed, for example, by neutron diffraction.
[0403] The O3' type crystal structure is CoO 2 CdCl with random lithium intercalated between layers 2 It can be said that this crystal structure is similar to that of the CdCl type. 2 A similar crystal structure to the Li-type is lithium nickel oxide. 0.06 NiO 2 The crystal structure is similar to that when charged to 1000V, but pure lithium cobaltate or layered rock salt-type positive electrode active materials containing a large amount of cobalt usually have a CdCl 2 It is known that it does not have a typical crystal structure.
[0404] CoO 2 The additive element, for example, magnesium, which is randomly and dilutely present between the layers, i.e., at the lithium site, turns into CoO when charged at a high voltage. 2 This has the effect of suppressing layer misalignment. 2 When magnesium is present between layers, an O3'-type crystal structure is likely to be formed. Therefore, magnesium is preferably distributed in at least the surface layer portion of the positive electrode active material 100 of one embodiment of the present invention, and further distributed throughout the positive electrode active material 100. In order to distribute magnesium throughout the positive electrode active material 100, heat treatment is preferably performed in the process of manufacturing the positive electrode active material 100 of one embodiment of the present invention.
[0405] However, if the heat treatment temperature is too high, cation mixing occurs, increasing the possibility that an added element, such as magnesium, will enter the cobalt site. Magnesium present in the cobalt site is ineffective in maintaining the R-3m structure during high-voltage charging. Furthermore, if the heat treatment temperature is too high, there are concerns about adverse effects such as cobalt being reduced to divalent and lithium transpiration.
[0406] Therefore, it is preferable to add a halogen compound such as a fluorine compound to the lithium cobalt oxide before the heat treatment for distributing magnesium in the positive electrode active material 100. Adding the halogen compound lowers the melting point of the lithium cobalt oxide. Lowering the melting point makes it easier to distribute magnesium in the positive electrode active material 100 at a temperature where cation mixing is unlikely to occur. Furthermore, the presence of a fluorine compound is expected to improve corrosion resistance against hydrofluoric acid produced by decomposition of the electrolyte.
[0407] Note that increasing the magnesium concentration above a desired value may reduce the effect on stabilizing the crystal structure. This is thought to be because magnesium enters the cobalt site in addition to the lithium site. The number of magnesium atoms in the positive electrode active material of one embodiment of the present invention is preferably 0.001 to 0.1 times the number of atoms of the transition metal, such as cobalt, more preferably more than 0.01 to less than 0.04 times, and even more preferably about 0.02 times. The magnesium concentration shown here may be, for example, a value obtained by elemental analysis of the entire particle of the positive electrode active material 100 using ICP-MS or the like, or may be based on the value of the raw material composition during the production process of the positive electrode active material.
[0408] Lithium cobalt oxide may contain one or more metals other than cobalt (hereinafter referred to as metal Z), such as nickel, aluminum, manganese, titanium, vanadium, and chromium. Adding one or more of nickel and aluminum is particularly preferred. Manganese, titanium, vanadium, and chromium may be stable and easily tetravalent, which may contribute significantly to structural stability. Adding metal Z may make the crystal structure more stable in a charged state at a high voltage. In the positive electrode active material of one embodiment of the present invention, metal Z is preferably added at a concentration that does not significantly change the crystallinity of lithium cobalt oxide. For example, the amount is preferably such that the aforementioned Jahn-Teller effect or the like is not exhibited.
[0409] The transition metals, including nickel and manganese, and aluminum are preferably present at the cobalt site, but may be partially present at the lithium site. Magnesium is preferably present at the lithium site. Oxygen may be partially substituted with fluorine.
[0410] As the magnesium concentration in the positive electrode active material of one embodiment of the present invention increases, the capacity of the positive electrode active material may decrease. One possible cause of this is the incorporation of magnesium into lithium sites, which may reduce the amount of lithium contributing to charge and discharge. Excess magnesium may also produce magnesium compounds that do not contribute to charge and discharge. When the positive electrode active material of one embodiment of the present invention contains nickel as the metal Z in addition to magnesium, the capacity per weight and per volume may be increased. When the positive electrode active material of one embodiment of the present invention contains aluminum as the metal Z in addition to magnesium, the capacity per weight and per volume may be increased. When the positive electrode active material of one embodiment of the present invention contains nickel and aluminum in addition to magnesium, the capacity per weight and per volume may be increased.
[0411] The concentrations of elements such as magnesium and metal Z contained in the positive electrode active material of one embodiment of the present invention will be discussed below.
[0412] When the positive electrode active material of one embodiment of the present invention contains magnesium in addition to element X, the stability in a high-voltage charged state is extremely high. When element X is phosphorus, the number of phosphorus atoms is preferably 1% to 20% of the number of cobalt atoms, more preferably 2% to 10%, and even more preferably 3% to 8%. In addition, the number of magnesium atoms is preferably 0.1% to 10%, more preferably 0.5% to 5%, and even more preferably 0.7% to 4% of the number of cobalt atoms. The concentrations of phosphorus and magnesium shown here may be values obtained by elemental analysis of the entire particles of the positive electrode active material using, for example, ICP-MS, or may be based on values of the composition of raw materials in the process of producing the positive electrode active material.
[0413] The number of nickel atoms in the positive electrode active material of one embodiment of the present invention is preferably 10% or less of the number of cobalt atoms, more preferably 7.5% or less, even more preferably 0.05% or more and 4% or less, and particularly preferably 0.1% or more and 2% or less. The nickel concentration shown here may be, for example, a value obtained by elemental analysis of the entire particles of the positive electrode active material using ICP-MS or the like, or may be based on the value of the composition of raw materials in the process of producing the positive electrode active material.
[0414] If the positive electrode active material 100 is charged at a high voltage for a long period of time, transition metals may leach out of the positive electrode active material into the electrolyte, causing the crystal structure to collapse. However, by containing nickel in the above proportions, it may be possible to suppress the leach-out of transition metals from the positive electrode active material 100.
[0415] The number of aluminum atoms in the positive electrode active material of one embodiment of the present invention is preferably 0.05% to 4%, and more preferably 0.1% to 2%, of the number of cobalt atoms. The aluminum concentration shown here may be a value obtained by elemental analysis of the entire particles of the positive electrode active material using, for example, ICP-MS or the like, or may be based on the value of the composition of raw materials in the process of producing the positive electrode active material.
[0416] The positive electrode active material of one embodiment of the present invention preferably contains an element X, and phosphorus is preferably used as the element X. Furthermore, the positive electrode active material of one embodiment of the present invention more preferably contains a composite oxide containing phosphorus and oxygen.
[0417] When the positive electrode active material of one embodiment of the present invention includes a composite oxide containing element X, a short circuit may be less likely to occur when the positive electrode active material is maintained in a charged state at a high voltage.
[0418] When the positive electrode active material of one embodiment of the present invention contains phosphorus as the element X, hydrogen fluoride generated by decomposition of the electrolyte solution may react with the phosphorus, resulting in a decrease in the hydrogen fluoride concentration in the electrolyte solution.
[0419] The electrolyte is LiPF as a lithium salt. 6In the case where the electrolyte contains PVDF, hydrogen fluoride may be generated by hydrolysis. Hydrogen fluoride may also be generated by the reaction of PVDF, which is used as a component of the positive electrode, with an alkali. By reducing the hydrogen fluoride concentration in the electrolyte, corrosion of the current collector and / or peeling of the coating may be suppressed. Furthermore, gelation and / or insolubilization of PVDF may be suppressed, which may result in a decrease in adhesion.
[0420] When the positive electrode active material has cracks, the presence of phosphorus, more specifically, a composite oxide containing phosphorus and oxygen, inside the cracks may inhibit the progression of the cracks.
[0421] As is clear from the oxygen atoms indicated by the arrows in Figure 18, the symmetry of the oxygen atoms is slightly different between the O3 type crystal structure and the O3' type crystal structure. Specifically, in the O3 type crystal structure, the oxygen atoms are aligned along the dotted line, whereas in the O3' type crystal structure, the oxygen atoms are not aligned strictly. This is because in the O3' type crystal structure, as lithium decreases, tetravalent cobalt increases, causing Jahn-Teller distortion to increase, resulting in CoO 6 This is because the octahedral structure of CoO is distorted. 2 Another factor is the increased repulsion between oxygen atoms in the layers.
[0422] <<Surface Layer 100a>> Magnesium is preferably distributed throughout the particle of the positive electrode active material 100 of one embodiment of the present invention, and in addition, the magnesium concentration in the surface layer 100a is preferably higher than the average magnesium concentration throughout the particle. For example, the magnesium concentration in the surface layer 100a measured by XPS or the like is preferably higher than the average magnesium concentration throughout the particle measured by ICP-MS or the like.
[0423] Furthermore, when the cathode active material 100 of one embodiment of the present invention contains an element other than cobalt, for example, one or more metals selected from nickel, aluminum, manganese, iron, and chromium, the concentration of the metal near the particle surface is preferably higher than the average concentration of the entire particle. For example, the concentration of the element other than cobalt in the surface layer 100 a measured by XPS or the like is preferably higher than the average concentration of the element in the entire particle measured by ICP-MS or the like.
[0424] The surface layer of the positive electrode active material is, so to speak, entirely composed of crystal defects. Furthermore, lithium is released from the surface during charging, making this portion prone to a lower lithium concentration than the interior. This makes the surface unstable and prone to collapse of the crystal structure. A high magnesium concentration in the surface layer 100a can more effectively suppress changes in the crystal structure. Furthermore, a high magnesium concentration in the surface layer 100a can be expected to improve corrosion resistance to hydrofluoric acid produced by decomposition of the electrolyte.
[0425] Furthermore, the concentration of halogen such as fluorine in the surface layer portion 100a of the positive electrode active material 100 of one embodiment of the present invention is preferably higher than the average concentration in the entire positive electrode active material 100. The presence of halogen in the surface layer portion 100a, which is the region in contact with the electrolyte, can effectively improve corrosion resistance to hydrofluoric acid.
[0426] As described above, the surface layer portion 100a of the cathode active material 100 of one embodiment of the present invention preferably has a different composition from the interior portion 100b, i.e., a higher concentration of additive elements, such as magnesium and fluorine, than the interior portion 100b. Furthermore, the composition preferably has a stable crystal structure at room temperature. Therefore, the surface layer portion 100a may have a different crystal structure from the interior portion 100b. For example, at least a portion of the surface layer portion 100a of the cathode active material 100 of one embodiment of the present invention may have a rock salt crystal structure. Furthermore, when the surface layer portion 100a and the interior portion 100b have different crystal structures, it is preferable that the crystal orientations of the surface layer portion 100a and the interior portion 100b roughly match.
[0427] The anions in the layered rock salt crystal and the rock salt crystal have a cubic close-packed structure (face-centered cubic lattice structure). It is estimated that the anions in the O3'-type crystal also have a cubic close-packed structure. When they contact, there is a crystal plane where the orientation of the cubic close-packed structure formed by the anions is aligned. However, the space group of the layered rock salt crystal and the O3'-type crystal is R-3m, which is different from the space group of the rock salt crystal, Fm-3m (the space group of a general rock salt crystal) and Fd-3m (the space group of a rock salt crystal with the simplest symmetry). Therefore, the Miller indices of the crystal planes that satisfy the above conditions are different between the layered rock salt crystal and the O3'-type crystal and the rock salt crystal. In this specification, when the orientation of the cubic close-packed structure formed by the anions is aligned in the layered rock salt crystal, the O3'-type crystal, and the rock salt crystal, the crystal orientation may be said to be approximately aligned.
[0428] The fact that the crystal orientations of the two regions roughly match can be determined from TEM (transmission electron microscope) images, STEM (scanning transmission electron microscope) images, HAADF-STEM (high-angle annular dark-field scanning transmission electron microscope) images, ABF-STEM (annular bright-field scanning transmission electron microscope) images, etc. X-ray diffraction (XRD), electron beam diffraction, neutron beam diffraction, etc. can also be used as materials for determination. When the crystal orientations roughly match, it can be observed in TEM images, etc. that the difference in direction between the rows of linearly alternating cations and anions is 5 degrees or less, more preferably 2.5 degrees or less. Note that light elements such as oxygen and fluorine may not be clearly observed in TEM images, etc., but in such cases, the alignment of the orientations can be determined from the arrangement of metal elements.
[0429] However, if the surface layer 100a is composed of only MgO or only a solid solution of MgO and CoO(II), it becomes difficult to insert and extract lithium. Therefore, the surface layer 100a must contain at least cobalt, and in a discharged state, it must also contain lithium, providing a path for lithium insertion and extraction. It is also preferable that the concentration of cobalt is higher than that of magnesium.
[0430] The element X is preferably located in the surface layer portion 100a of the positive electrode active material 100 of one embodiment of the present invention. For example, the positive electrode active material 100 of one embodiment of the present invention may be covered with a coating (barrier layer) containing the element X.
[0431] <Grain Boundary> The additional element X contained in the positive electrode active material 100 of one embodiment of the present invention may be present randomly and dilutely inside the positive electrode active material 100, but more preferably, a part of the additional element X segregates at the grain boundary.
[0432] In other words, the concentration of the additional element X at and near the grain boundaries of the positive electrode active material 100 of one embodiment of the present invention is preferably higher than that in other regions inside the grain boundaries.
[0433] Like the particle surfaces, the grain boundaries are also planar defects. Therefore, they are prone to instability and changes in the crystal structure are likely to occur. Therefore, if the concentration of the added element X at and near the grain boundaries is high, changes in the crystal structure can be more effectively suppressed.
[0434] Furthermore, when the concentration of the additive element X is high at and near the grain boundary, even if cracks occur along the grain boundary of the positive electrode active material 100 of one embodiment of the present invention, the concentration of the additive element X becomes high near the surface where the cracks occur. Therefore, the corrosion resistance to hydrofluoric acid can be improved even in the positive electrode active material after the cracks occur.
[0435] In this specification and the like, the vicinity of the grain boundary refers to the region up to about 10 nm from the grain boundary.
[0436] <<Particle size>> If the particle size of the positive electrode active material 100 of one embodiment of the present invention is too large, problems such as difficulty in diffusing lithium or excessive roughness of the surface of the active material layer when applied to a current collector occur. On the other hand, if the particle size is too small, problems such as difficulty in supporting the active material layer when applied to a current collector or excessive reaction with an electrolyte solution occur. Therefore, the average particle size (D50: also referred to as median diameter) is preferably 1 μm or more and 100 μm or less, more preferably 2 μm or more and 40 μm or less, and even more preferably 5 μm or more and 30 μm or less.
[0437] <Analysis Method> Whether a certain cathode active material is the cathode active material 100 of one embodiment of the present invention that exhibits an O3'-type crystal structure when charged at a high voltage can be determined by analyzing the cathode charged at a high voltage using XRD, electron diffraction, neutron diffraction, electron spin resonance (ESR), nuclear magnetic resonance (NMR), etc. XRD is particularly preferred in that it can analyze the symmetry of transition metals such as cobalt contained in the cathode active material with high resolution, it can compare the level of crystallinity and the orientation of the crystals, it can analyze the periodic distortion of the lattice and the crystallite size, and it can obtain sufficient accuracy even when measuring a cathode obtained by disassembling a secondary battery as is.
[0438] As described above, the cathode active material 100 of one embodiment of the present invention is characterized by minimal change in crystal structure between a high-voltage charged state and a discharged state. Materials in which a crystal structure that exhibits a significant change between a high-voltage charged state and a discharged state accounts for 50 wt % or more are undesirable because they cannot withstand high-voltage charging and discharging. It should be noted that the desired crystal structure may not be achieved simply by adding an additive element. For example, even if both materials share the common feature of being lithium cobalt oxide containing magnesium and fluorine, there are cases in which the O3'-type crystal structure accounts for 60 wt % or more and cases in which the H1-3-type crystal structure accounts for 50 wt % or more when charged at a high voltage. Furthermore, at a certain voltage, the O3'-type crystal structure may be nearly 100 wt %, and further increasing the certain voltage may result in the H1-3-type crystal structure. Therefore, to determine whether a material is the cathode active material 100 of one embodiment of the present invention, analysis of the crystal structure, such as XRD, is required.
[0439] However, when a positive electrode active material is charged or discharged at a high voltage, its crystal structure may change when exposed to air. For example, it may change from an O3'-type crystal structure to an H1-3-type crystal structure. Therefore, it is preferable to handle all samples in an inert atmosphere such as an argon atmosphere.
[0440] <Charging Method> High-voltage charging for determining whether a certain composite oxide is the positive electrode active material 100 of one embodiment of the present invention can be performed, for example, by preparing a coin cell (CR2032 type, diameter 20 mm, height 3.2 mm) using a lithium counter electrode.
[0441] More specifically, the positive electrode may be prepared by coating a positive electrode current collector made of aluminum foil with a slurry containing a positive electrode active material and a conductive agent.
[0442] Lithium metal can be used for the counter electrode. When a material other than lithium metal is used for the counter electrode, the potential of the secondary battery differs from the potential of the positive electrode. Unless otherwise specified, voltages and potentials in this specification refer to the potential of the positive electrode.
[0443] The electrolyte contained in the electrolytic solution was 1 mol / L lithium hexafluorophosphate (LiPF 6 ) is used, and the electrolyte may be a mixture of ethylene carbonate (EC) and diethyl carbonate (DEC) in a volume ratio of EC:DEC=3:7 with 2 wt % vinylene carbonate (VC).
[0444] The separator can be made of polypropylene having a thickness of 25 μm.
[0445] The positive electrode can and the negative electrode can may be made of stainless steel (SUS).
[0446] The coin cell prepared under the above conditions is charged at a constant current of 4.6 V and 0.5 C, and then charged at a constant voltage until the current reaches 0.01 C. Here, 1 C is 200 mA / g. The temperature is 25°C. After charging in this manner, the coin cell is disassembled in an argon-atmosphere glove box and the positive electrode is removed to obtain a positive electrode active material charged at a high voltage. When various analyses are performed after this, it is preferable to seal the cell in an argon atmosphere to prevent reactions with external components. For example, XRD can be performed by sealing the cell in an airtight container in an argon atmosphere.
[0447] <XRD> Figures 19 and 21 show ideal powder XRD patterns calculated from the O3'-type crystal structure and H1-3-type crystal structure models using CuKα1 radiation. x CoO 2 LiCoO where x=1 2 The ideal XRD patterns calculated from the crystal structures of O3, H1-3 type, and trigonal O1 with x = 0 are also shown. 2 O3 and CoO 2 The O1 pattern was created using Reflex Powder Diffraction, a module of Materials Studio (BIOVIA), from crystal structure information obtained from the Inorganic Crystal Structure Database (ICSD) (see Non-Patent Document 5). The 2θ range was 15° to 75°, with a step size of 0.01 and a wavelength of λ1 of 1.540562 × 10. −10 m and λ2 were not set, and the monochromator was single. The pattern of the H1-3 type crystal structure was similarly created from the crystal structure information described in Non-Patent Document 3. The pattern of the O3' type crystal structure was created by estimating the crystal structure from the XRD pattern of the positive electrode active material of one embodiment of the present invention and fitting it using TOPAS ver. 3 (crystal structure analysis software manufactured by Bruker), and an XRD pattern was created in the same manner as the others.
[0448] As shown in Figure 19, in the O3' type crystal structure, diffraction peaks appear at 2θ = 19.30 ± 0.20° (19.10° to 19.50°) and 2θ = 45.55 ± 0.10° (45.45° to 45.65°). More specifically, sharp diffraction peaks appear at 2θ = 19.30 ± 0.10° (19.20° to 19.40°) and 2θ = 45.55 ± 0.05° (45.50° to 45.60°). However, as shown in Figure 21, in the H1-3 type crystal structure and CoO 2 No peaks appear at these positions in O1. Therefore, the appearance of peaks at 2θ = 19.30 ± 0.20° and 2θ = 45.55 ± 0.10° in a state charged at a high voltage can be said to be a characteristic of the positive electrode active material 100 of one embodiment of the present invention.
[0449] This means that the positions at which XRD diffraction peaks appear are close between x = 1 and x ≦ 0.24. More specifically, the difference in the positions at which two or more, preferably three or more, of the main diffraction peaks of both samples is 2θ = 0.7 or less, more preferably 2θ = 0.5 or less.
[0450] Note that the positive electrode active material 100 of one embodiment of the present invention is LixCoO 2 When x in the formula is small, the cathode active material 100 has an O3'-type crystal structure, but not all of the cathode active material 100 has an O3'-type crystal structure. It may contain other crystal structures, or may be partially amorphous. However, when Rietveld analysis is performed on the XRD pattern, the O3'-type crystal structure is preferably 50 wt% or more, more preferably 60 wt% or more, and even more preferably 66 wt% or more. If the O3'-type crystal structure is 50 wt% or more, more preferably 60 wt% or more, and even more preferably 66 wt% or more, it can be a cathode active material with sufficiently excellent cycle characteristics.
[0451] Furthermore, even after 100 or more charge / discharge cycles from the start of cycle measurement, when Rietveld analysis is performed, the O3' type crystal structure is preferably 35 wt% or more, more preferably 40 wt% or more, and even more preferably 43 wt% or more.
[0452] The crystallite size of the O3'-type crystal structure of the positive electrode active material is 2 Therefore, even under the same XRD measurement conditions as the positive electrode before and after charging and discharging, the LixCoO 2 When x in the formula is small, a clear peak of the O3' type crystal structure can be confirmed. 2 In this case, even if a part of the crystal structure resembles the O3'-type crystal structure, the crystallite size will be small and the peak will be broad and small. The crystallite size can be determined from the half-width of the XRD peak.
[0453] As described above, the positive electrode active material of one embodiment of the present invention preferably has a small influence of the Jahn-Teller effect. The positive electrode active material of one embodiment of the present invention preferably has a layered rock salt crystal structure and contains cobalt as a transition metal. Furthermore, the positive electrode active material of one embodiment of the present invention may contain the above-described metal Z in addition to cobalt, as long as the influence of the Jahn-Teller effect is small.
[0454] In the positive electrode active material, the range of lattice constants in which the influence of the Jahn-Teller effect is presumed to be small will be considered using XRD analysis.
[0455] FIG. 22 shows the results of estimating the a-axis and c-axis lattice constants using XRD for a positive electrode active material of one embodiment of the present invention having a layered rock-salt crystal structure and containing cobalt and nickel. The positive electrode active material was prepared using steps S11 to S34 described below, with at least a nickel source used in step S21. FIG. 22A shows the a-axis results, and FIG. 22B shows the c-axis results. Note that FIGS. 22A and 22B show the results for the powder of positive electrode active material obtained according to steps S11 to S34. That is, the results are for the powder before being incorporated into a positive electrode. The nickel concentration (%) on the horizontal axis indicates the nickel concentration ratio (proportion) when the sum of the number of cobalt and nickel atoms is taken as 100%. The nickel concentration ratio (proportion) can be determined using a cobalt source and a nickel source.
[0456] FIG. 23 shows the results of estimating the a-axis and c-axis lattice constants using XRD patterns for a positive electrode active material of one embodiment of the present invention having a layered rock-salt crystal structure and containing cobalt and manganese. The positive electrode active material was prepared using steps S11 to S34 described below, with at least a manganese source used in step S21. FIG. 23A shows the a-axis results, and FIG. 23B shows the c-axis results. Note that FIGS. 23A and 23B show the results for the powder of positive electrode active material obtained according to steps S11 to S34. That is, the results are for the powder before being incorporated into a positive electrode. The manganese concentration (%) on the horizontal axis represents the concentration ratio (proportion) of manganese when the sum of the number of cobalt and manganese atoms is taken as 100%. The concentration ratio (proportion) of manganese can be determined using a cobalt source and a manganese source.
[0457] Fig. 22C shows the value obtained by dividing the a-axis lattice constant by the c-axis lattice constant (a-axis / c-axis) for the positive electrode active materials whose lattice constant results are shown in Fig. 22A and Fig. 22B. Fig. 23C shows the value obtained by dividing the a-axis lattice constant by the c-axis lattice constant (a-axis / c-axis) for the positive electrode active materials whose lattice constant results are shown in Fig. 23A and Fig. 23B.
[0458] 22C, a significant change in the a-axis / c-axis ratio is observed when the nickel concentration on the horizontal axis is 5% or 7.5%, which suggests that the distortion of the a-axis is large. This distortion may be Jahn-Teller distortion. This suggests that an excellent positive electrode active material with small Jahn-Teller distortion can be obtained when the nickel concentration is less than 7.5%.
[0459] Next, Figure 23A suggests that when the manganese concentration is 5% or more, the behavior of the change in lattice constant is different and does not follow Vegard's law. Therefore, it is suggested that when the manganese concentration is 5% or more, the crystal structure is different. Therefore, the manganese concentration is preferably, for example, 4% or less.
[0460] The above ranges of nickel concentration and manganese concentration do not necessarily apply to the surface layer 100a of the particle, that is, the surface layer 100a of the particle may have higher concentrations than the above ranges.
[0461] As a result of considering a preferable range of the lattice constant from the above, it was found that in the positive electrode active material of one embodiment of the present invention, the a-axis lattice constant is 2.814 × 10 in the layered rock salt crystal structure of the particles of the positive electrode active material in a state where no charge / discharge is performed or in a discharged state, which can be estimated from the XRD pattern. −10 m is greater than 2.817 x 10 −10 m and the lattice constant of the c-axis is 14.05 × 10 −10 m or larger, 14.07 x 10 −10 It has been found that it is preferable that the length be smaller than m. The state in which no charge or discharge is performed may be, for example, the state of powder before the positive electrode of a secondary battery is produced.
[0462] Alternatively, in the layered rock-salt crystal structure of the particles of the positive electrode active material in a state where no charge or discharge is performed or in a discharged state, it is preferable that the value obtained by dividing the lattice constant of the a-axis by the lattice constant of the c-axis (a-axis / c-axis) is greater than 0.20000 and smaller than 0.20049.
[0463] Alternatively, when XRD analysis is performed on a layered rock salt type crystal structure possessed by particles of a positive electrode active material in a state where no charge / discharge is performed or in a discharged state, a first peak may be observed at 2θ of not less than 18.50° and not more than 19.30°, and a second peak may be observed at 2θ of not less than 38.00° and not more than 38.80°.
[0464] The peaks appearing in the powder XRD pattern reflect the crystalline structure of the interior 100b of the positive electrode active material 100, which occupies the majority of the volume of the positive electrode active material 100. The crystalline structure of the surface layer 100a and the like can be analyzed by electron beam diffraction or the like of a cross section of the positive electrode active material 100.
[0465] <XPS> X-ray photoelectron spectroscopy (XPS) can analyze a region from the surface to a depth of 2 nm to 8 nm (usually about 5 nm), so the concentration of each element can be quantitatively analyzed for about half of the surface layer 100a. Furthermore, narrow scan analysis can be used to analyze the bonding state of elements. The quantitative accuracy of XPS is often about ±1 atomic %, and the lower detection limit is about 1 atomic %, depending on the element.
[0466] When XPS analysis was performed on the positive electrode active material 100 of one embodiment of the present invention, the number of atoms of the additive element was preferably 1.6 to 6.0 times, and more preferably 1.8 to less than 4.0 times, the number of atoms of the transition metal. When the additive element is magnesium and the transition metal is cobalt, the number of magnesium atoms was preferably 1.6 to 6.0 times, and more preferably 1.8 to less than 4.0 times, the number of atoms of cobalt. Furthermore, the number of atoms of the halogen such as fluorine was preferably 0.2 to 6.0 times, and more preferably 1.2 to 4.0 times, the number of atoms of the transition metal.
[0467] When XPS analysis is performed, for example, monochromated aluminum can be used as the X-ray source, and the take-off angle can be set to, for example, 45°.
[0468] Furthermore, when the positive electrode active material 100 of one embodiment of the present invention is subjected to XPS analysis, the peak representing the bond energy between fluorine and another element is preferably equal to or greater than 682 eV and less than 685 eV, and more preferably about 684.3 eV. This value is different from both the bond energy of lithium fluoride (685 eV) and the bond energy of magnesium fluoride (686 eV). In other words, when the positive electrode active material 100 of one embodiment of the present invention contains fluorine, the bond is preferably other than that of lithium fluoride or magnesium fluoride.
[0469] Furthermore, when the positive electrode active material 100 of one embodiment of the present invention is subjected to XPS analysis, the peak representing the bond energy between magnesium and another element is preferably equal to or greater than 1302 eV and less than 1304 eV, and more preferably about 1303 eV. This value is different from the bond energy of magnesium fluoride, 1305 eV, and is close to the bond energy of magnesium oxide. In other words, when the positive electrode active material 100 of one embodiment of the present invention contains magnesium, the bond is preferably other than that of magnesium fluoride.
[0470] The concentration of the added element, such as magnesium or aluminum, which is preferably present in large amounts in the surface layer portion 100a, measured by XPS or the like is preferably higher than the concentration measured by ICP-MS (inductively coupled plasma mass spectrometry) or GD-MS (glow discharge mass spectrometry).
[0471] When a cross section of magnesium or aluminum is exposed by processing and analyzed using TEM-EDX, the concentration of the surface layer 100 a is preferably higher than the concentration of the inner layer 100 b. The processing can be performed using, for example, a focused ion beam (FIB).
[0472] In an XPS (X-ray photoelectron spectroscopy) analysis, the number of magnesium atoms is preferably 0.4 to 1.5 times the number of cobalt atoms, while in an ICP-MS analysis, the ratio of the number of magnesium atoms, Mg / Co, is preferably 0.001 to 0.06.
[0473] On the other hand, it is preferable that nickel contained in the transition metal is not unevenly distributed in the surface layer portion 100a but is distributed throughout the positive electrode active material 100. However, this does not apply when there is a region where the excess additive element is unevenly distributed as described above.
[0474] <Charge curve and dQ / dV curve> A non-equilibrium phase change occurs around the peak in the dQ / dV curve obtained by differentiating (dQ / dV) the capacity (Q) from the charge curve with respect to the voltage (V), and it is believed that the crystal structure changes significantly. In this specification, a non-equilibrium phase change refers to a phenomenon that causes a non-linear change in a physical quantity.
[0475] FIG. 24 shows charge curves of a secondary battery including a positive electrode active material of one embodiment of the present invention and a secondary battery including a positive electrode active material of a comparative example.
[0476] The positive electrode active material 1 of the present invention shown in FIG. 24 was produced by the production method shown in FIGS. 14A and 14B. More specifically, the LiMO 2 Lithium cobalt oxide (C-10N manufactured by Nippon Chemical Industry Co., Ltd.) was used as the 2Using this positive electrode active material, a half cell was prepared and charged in the same manner as in the XRD measurement.
[0477] The positive electrode active material 2 of the present invention shown in FIG. 24 was produced by the production method shown in FIGS. 14A and 14C. More specifically, the LiMO 2 Lithium cobalt oxide (C-10N manufactured by Nippon Chemical Industry Co., Ltd.) was used as the 2 , Ni(OH) 2 and Al(OH) 3 Using this positive electrode active material, a half cell was prepared and charged in the same manner as in the XRD measurement.
[0478] The positive electrode active material of the comparative example in Fig. 24 was prepared by forming an aluminum-containing layer on the surface of lithium cobalt oxide (C-5H manufactured by Nippon Chemical Industry Co., Ltd.) by a sol-gel method, followed by heating at 500°C for 2 hours. Using this positive electrode active material, a half cell was prepared and charged in the same manner as in the XRD measurement.
[0479] 24 shows the charging curves when these half-cells were charged at 10 mA / g up to 4.9 V at 25° C. For positive electrode active material 1 and the comparative example, n=2, and for positive electrode active material 2, n=1.
[0480] 25A to 25C show dQ / dV curves, which represent the amount of change in voltage with respect to charge capacity, obtained from the data in Fig. 24. Fig. 25A shows the dQ / dV curve for a half cell using positive electrode active material 1 of one embodiment of the present invention, Fig. 25B shows the dQ / dV curve for a half cell using positive electrode active material 2 of one embodiment of the present invention, and Fig. 25C shows the dQ / dV curve for a half cell using a positive electrode active material of a comparative example.
[0481] As is clear from Figures 25A to 25C, in both the embodiment of the present invention and the comparative example, peaks were observed at voltages of about 4.06 V and about 4.18 V, and the change in capacity with respect to voltage was nonlinear. x CoO 2 It is believed that the crystal structure (space group P2 / m) is when x is 0.5. x CoO 2In the space group P2 / m where x is 0.5, lithium atoms are aligned as shown in Figure 20. It is thought that energy is consumed for this alignment of lithium atoms, resulting in a nonlinear change in capacity with voltage.
[0482] 25C, large peaks were observed at approximately 4.54 V and 4.61 V. The region between these two peaks is considered to represent an H1-3 phase type crystal structure.
[0483] On the other hand, in the secondary battery of one embodiment of the present invention shown in FIGS. 25A and 25B , which exhibits extremely good cycle characteristics, a small peak was observed at about 4.55 V, but it was not clear. Furthermore, in the case of cathode active material 2, no subsequent peak was observed even above 4.7 V, indicating that the O3′ structure was maintained. As described above, in the dQ / dV curve of a secondary battery using the cathode active material of one embodiment of the present invention, some peaks may be extremely broad or small at 25° C. In such cases, two crystal structures may coexist. For example, two phases, O3 and O3′, or two phases, O3′ and H1-3, may coexist.
[0484] <Discharge Curve and dQ / dV Curve> Furthermore, when the positive electrode active material of one embodiment of the present invention is charged at a high voltage and then discharged at a low rate of, for example, 0.2 C or less, a characteristic voltage change may appear near the end of discharge. This change can be clearly confirmed by the presence of at least one peak in the voltage range up to 3.5 V, which is lower than the peak that appears around 3.9 V, in the dQ / dV curve obtained from the discharge curve.
[0485] <Surface Roughness and Specific Surface Area> The positive electrode active material 100 of one embodiment of the present invention preferably has a smooth surface with few irregularities. A smooth surface with few irregularities is one factor indicating that the distribution of the additive element in the surface layer portion 100 a is good.
[0486] Whether the surface is smooth and has few irregularities can be determined from, for example, a cross-sectional SEM image or cross-sectional TEM image of the positive electrode active material 100, the specific surface area of the positive electrode active material 100, or the like.
[0487] For example, the surface smoothness can be quantified from a cross-sectional SEM image of the positive electrode active material 100 as follows.
[0488] First, the cathode active material 100 is processed using an FIB or the like to expose a cross section. At this time, it is preferable to cover the cathode active material 100 with a protective film, protective agent, or the like. Next, an SEM image of the interface between the protective film or the like and the cathode active material 100 is taken. The SEM image is subjected to noise processing using image processing software. For example, Gaussian blurring (σ = 2) is performed, followed by binarization. Furthermore, interface extraction is performed using image processing software. Furthermore, the interface line between the protective film or the like and the cathode active material 100 is selected using a magic hand tool or the like, and the data is extracted into a spreadsheet software or the like. Using the functions of the spreadsheet software or the like, correction is performed from the regression curve (quadratic regression), and parameters for calculating roughness are obtained from the data after slope correction, and the root mean square surface roughness (RMS) is calculated from the standard deviation. Furthermore, this surface roughness is the surface roughness at least within 400 nm of the outer periphery of the particle of the cathode active material.
[0489] On the particle surfaces of the positive electrode active material 100 of the present embodiment, the roughness (RMS root mean square surface roughness), which is an index of roughness, is preferably less than 3 nm, more preferably less than 1 nm, and even more preferably less than 0.5 nm.
[0490] The image processing software used for noise processing, boundary extraction, etc. is not particularly limited, but for example, "ImageJ" can be used. The spreadsheet software is also not particularly limited, but for example, Microsoft Office Excel can be used.
[0491] For example, the actual specific surface area A measured by the gas adsorption method using the constant volume method R and the ideal specific surface area A i The smoothness of the surface of the positive electrode active material 100 can also be quantified from the ratio of
[0492] Ideal specific surface area A i is calculated assuming that all particles have the same diameter as D50, the same weight, and an ideal spherical shape.
[0493] The median diameter D50 can be measured by a particle size distribution analyzer using a laser diffraction / scattering method, etc. The specific surface area can be measured by a specific surface area measuring device using a gas adsorption method based on a constant volume method, for example.
[0494] The positive electrode active material 100 according to one embodiment of the present invention has an ideal specific surface area A calculated from the median diameter D50. i and the actual specific surface area A R Ratio A R / A i is preferably 2 or less.
[0495] [Defects in Positive Electrode Active Material] Examples of defects that may occur in a positive electrode active material are shown in Figures 26 to 36. Note that the positive electrode active material of one embodiment of the present invention is expected to have the effect of suppressing the occurrence of such defects.
[0496] Charging and discharging under high voltage conditions of 4.5 V or higher or at high temperatures (45°C or higher) can cause progressive defects such as pits in the positive electrode active material. Furthermore, cracks can also occur due to the expansion and contraction of the positive electrode active material during charging and discharging. Figure 26 shows a schematic cross-sectional view of a positive electrode active material 51. In the positive electrode active material 51, pits 54 and 58 are illustrated as holes, but the openings are not circular but have depth. The positive electrode active material 51 may also have cracks 57. The positive electrode active material 51 has crystal faces 55 and may also have recesses 52. Barrier layers 53 and 56 preferably cover the positive electrode active material 51, but may also be separated. The barrier layer 53 also covers the recesses 52.
[0497] The positive electrode active material of a lithium-ion secondary battery is typically LCO or NCM, which can also be considered an alloy containing multiple metal elements (e.g., cobalt, nickel, etc.). At least one of the multiple positive electrode active materials may have defects, and the defects may change before and after charge and discharge. When used in a secondary battery, the positive electrode active material may be chemically or electrochemically eroded by the environmental substances surrounding the positive electrode active material (e.g., electrolyte), or the material may deteriorate. This deterioration does not occur uniformly on the surface of the positive electrode active material, but occurs in a locally concentrated manner, and repeated charge and discharge of the secondary battery may cause defects to form deep from the surface to the interior, for example.
[0498] The phenomenon in which defects progress and form holes in the positive electrode active material may be called pitting corrosion.
[0499] In this specification, cracks and pits are different. Immediately after the preparation of the positive electrode active material, cracks are present but pits are not. Pits are holes formed by the loss of several layers of cobalt or oxygen due to charging and discharging under high voltage conditions of 4.5 V or higher or at high temperatures (45°C or higher), and can also be considered as locations where cobalt has dissolved. Therefore, pits are not present immediately after the preparation of the positive electrode active material. Cracks refer to new surfaces formed by the application of physical pressure or cracks caused by grain boundaries. Cracks may also occur due to particle expansion and contraction caused by charging and discharging. Pits may also occur from cracks or cavities within particles.
[0500] <Disassembly of Secondary Battery> A charge / discharge test was performed up to 50 cycles. The discharge capacity at the 50th cycle was reduced to less than 40% of that at the first cycle. The secondary battery was disassembled, and the positive electrode was removed. Disassembly was performed under an argon atmosphere. After disassembly, the battery was washed with DMC, and the solvent was then evaporated. Observations were made on the positive electrode that had undergone the charge / discharge test up to 50 cycles, and the positive electrode before incorporation into the secondary battery, i.e., the positive electrode immediately after fabrication.
[0501] <SEM Observation> The positive electrode was observed using a scanning electron microscope (SEM). Fig. 27A shows an SEM image of the positive electrode of the secondary battery after 50 cycles. Fig. 27B shows an SEM image of the positive electrode before incorporation into the secondary battery. A scanning electron microscope SU8030 manufactured by Hitachi High-Tech Corporation was used for the SEM observation.
[0502] Next, the cathode active material was cross-sectionally processed using an FIB, and the cross-section of the cathode active material was observed using an SEM. By repeating cross-sectional processing using an FIB and SEM observation, three-dimensional information on the structure shown in FIG. 28A or 28D can be obtained. Note that a Hitachi High-Tech XVision 210B was used for FIB processing and SEM observation.
[0503] Fig. 28B is a partially enlarged view of the three-dimensional information in Fig. 28A from the front, and Fig. 28C shows a cross-sectional view of the same. Fig. 28D corresponds to the three-dimensional information of the side view obtained by rotating the three-dimensional information in Fig. 28A. Fig. 28E is a partially enlarged view of Fig. 28D, and Fig. 28F shows a cross-sectional view of the same. As shown in Fig. 28F, the pits are not holes, but have a shape that can also be called grooves or fissures having a width.
[0504] Fig. 29A shows an SEM image of the upper surface of the positive electrode of a secondary battery after 50 cycles. Fig. 29B is a cross-sectional view of the dashed line portion in Fig. 29A. Fig. 29C is an enlarged view of the rectangular framed portion in Fig. 29B. Fig. 29C shows pits 90a, 90b, and 90c.
[0505] Fig. 30A shows an SEM image of the top surface of the positive electrode before it is incorporated into a secondary battery. Fig. 30B is a cross-sectional view of the dashed line portion in Fig. 30A. Fig. 30C is an enlarged view of the portion enclosed by the square frame in Fig. 30B. Fig. 30C shows a crack 91b.
[0506] As described above, when the positive electrode was observed after 50 cycles, pits and cracks were observed.
[0507] <STEM Observation> Next, the cross section of the positive electrode of the secondary battery after 50 cycles was observed by a scanning transmission electron microscope (STEM). The sample for cross section observation was processed using an FIB.
[0508] <EDX Analysis> The positive electrode of the secondary battery after 50 cycles was evaluated using energy dispersive X-ray spectroscopy (EDX).
[0509] Fig. 31A shows a cross-sectional STEM image of the positive electrode, and Fig. 31B is an enlarged view of the area enclosed by the square frame in Fig. 31A.
[0510] EDX mapping of the region shown in FIG. 31B is shown in FIGS. 32A to 32C. FIG. 32A shows EDX mapping of magnesium, FIG. 32B shows EDX mapping of aluminum, and FIG. 32C shows EDX mapping of cobalt. A Hitachi High-Tech HD-2700 was used for the EDX analysis. The acceleration voltage was 200 kV. The EDX mapping suggested that magnesium and aluminum were present in at least a portion of the surface layer of the particles of the positive electrode active material.
[0511] <Micro-electron diffraction> Next, the crystal structure of the grain boundaries of the lithium cobalt oxide and the vicinity thereof was analyzed using micro-electron diffraction.
[0512] Figure 33A is a cross-sectional TEM image of degraded lithium cobalt oxide after 50 cycles. Figure 33B is an enlarged image of the area surrounded by the black line in Figure 33A. The analysis points of the electron microbeam diffraction are indicated by stars NBED1, NBED2, and NBED3 in Figure 33B.
[0513] Figure 34A shows the electron microbeam diffraction pattern of the star NBED1 portion. The transmitted light is O, and some of the diffraction spots are shown in the figure as DIFF1-1, DIFF1-2, and DIFF1-3. When the star NBED1 portion was analyzed, the lattice spacing of DIFF1-1 was calculated to be 0.475 nm, the lattice spacing of DIFF1-2 was 0.199 nm, and the lattice spacing of DIFF1-3 was calculated to be 0.238 nm. The plane angles were also ∠1O2 = 55 °, ∠1O3 = 80 °, and ∠2O3 = 24 °. In this case, the electron beam incident direction is [0-10], and from the plane spacing and plane angle, DIFF1-1 is 10-2 of the layered rock salt crystal, DIFF1-2 is 10-5 similarly, and DIFF1-3 is 00-3 similarly, and LiCoO 2 It was thought to have the following crystal structure.
[0514] FIG. 34B shows the electron microbeam diffraction pattern of the star-marked NBED2 portion. The transmitted light is O, and some of the diffraction spots are labeled DIFF2-1, DIFF2-2, and DIFF2-3, and are shown in the figure. Analysis of the star-marked NBED2 portion revealed that the interplanar spacing of DIFF2-1 was 0.468 nm, the interplanar spacing of DIFF2-2 was 0.398 nm, and the interplanar spacing of DIFF2-3 was 0.472 nm. The plane angles were ∠1O2 = 54°, ∠1O3 = 110°, and ∠2O3 = 56°. From the interplanar spacings and plane angles, DIFF2-1, DIFF2-2, and DIFF2-3 were spinel-type crystals, and Co 3 O 4 or LiCo 2 O 4 It was thought to have the following crystal structure.
[0515] Figure 34C shows the electron microbeam diffraction pattern of the star NBED3 portion. The transmitted light is O, and some of the diffraction spots are designated DIFF3-1, DIFF3-2, and DIFF3-3, and are shown in the figure. Analysis of the star NBED1 portion revealed that the lattice spacing of DIFF3-1 was 0.241 nm, the lattice spacing of DIFF3-2 was 0.210 nm, and the lattice spacing of DIFF3-3 was 0.246 nm. The plane angles were ∠1O2 = 55 °, ∠1O3 = 110 °, and ∠2O3 = 55 °. From the plane spacing and plane angle, it was thought that DIFF3-1, DIFF3-2, and DIFF3-3 were rock salt crystals and had a CoO crystal structure.
[0516] Figure 35A shows a layered rock salt structure, LiCoO 2 The crystal structure of LiCo is shown in Figure 35B. 2 O 4 Fig. 35C shows the crystal structure of CoO, which is a rock salt type.
[0517] 36A is a cross-sectional STEM image of a portion of a positive electrode active material layer after a current collector was coated with a slurry that would become the positive electrode active material layer and then pressed. Due to the pressing, steps were observed on the particle surfaces in the direction perpendicular to the lattice fringes (c-axis direction), and evidence of deformation along the lattice fringe direction (the ab-plane direction) was observed.
[0518] 36B is a schematic cross-sectional view of a particle before pressing. In the particle before pressing, a barrier layer is present relatively uniformly on the particle surface in the direction perpendicular to the lattice fringes.
[0519] 36C is a cross-sectional schematic diagram of a particle after pressing. The pressing process causes misalignment in the lattice fringe direction (the ab plane direction). The barrier layer also has multiple steps and is non-uniform. Regarding the misalignment in the ab plane direction, the particle surface opposite to the surface where the irregularities were observed also has irregularities of a similar shape, and some of the particles have misalignment in the ab plane direction.
[0520] The multiple steps shown in Figure 36C are observed as striped patterns on the particle surface. The striped patterns observed on the particle surface due to the steps caused by the displacement caused by pressing are called slips (stacking faults). Such particle slippage can cause the barrier layer to become non-uniform, which can lead to deterioration. Therefore, it is desirable to minimize or eliminate slippage of the positive electrode active material.
[0521] This embodiment mode can be implemented in appropriate combination with other embodiment modes.
[0522] Embodiment 4 In this embodiment, an example of a method for manufacturing a positive electrode active material of one embodiment of the present invention will be described with reference to FIGS.
[0523] [Method 1 for Manufacturing Positive Electrode Active Material] An example of a method for manufacturing a positive electrode active material according to one embodiment of the present invention will be described with reference to FIGS.
[0524] In step S21 of FIG. 37, a transition metal M1 source 800 is prepared.
[0525] The transition metal M1 may be, for example, at least one of manganese, cobalt, and nickel. For example, the transition metal M1 may be composed of only cobalt, only nickel, two metals, cobalt and manganese, two metals, cobalt and nickel, or three metals, cobalt, manganese, and nickel. The source of the transition metal M1 is prepared as an aqueous solution containing the transition metal M1.
[0526] As the transition metal M1 source 800, an aqueous solution containing cobalt such as an aqueous cobalt sulfate solution or an aqueous cobalt nitrate solution can be used, an aqueous solution containing nickel such as an aqueous nickel sulfate solution or an aqueous nickel nitrate solution can be used, and an aqueous solution containing manganese such as an aqueous manganese sulfate solution or an aqueous manganese nitrate solution can be used.
[0527] It is preferable to use a high-purity material as the transition metal M1 source 800 used in the synthesis. Specifically, when using an aqueous solution containing the transition metal M1, the purity of the solute material when preparing the aqueous solution is 2N (99%) or higher, preferably 3N (99.9%) or higher, and more preferably 4N (99.99%) or higher. The water is preferably pure water with a low impurity content, preferably with a resistivity of 1 MΩ cm or higher, more preferably 10 MΩ cm or higher, and even more preferably 15 MΩ cm or higher. The use of a high-purity material can increase the capacity and / or reliability of the secondary battery.
[0528] When using metals capable of forming a layered rock salt type composite oxide, it is preferable to set the mixing ratio of cobalt, manganese, and nickel within a range that allows a layered rock salt type crystal structure to be formed.
[0529] Next, in step S31, the transition metal M1 source 800 is mixed to obtain a mixture 811 in step S32.
[0530] Next, an aqueous solution A 812 is prepared in step S33, and an aqueous solution B 813 is prepared in step S34.
[0531] As the aqueous solution A812, one or a mixture of a solution containing at least one of chelating agents such as glycine, oxine, 1-nitroso-2-naphthol, or 2-mercaptobenzothiazole, or ammonia water can be used.
[0532] As the aqueous solution B813, any one of an aqueous solution of sodium hydroxide, an aqueous solution of potassium hydroxide, and an aqueous solution of lithium hydroxide, or a mixture of two or more thereof can be used.
[0533] Next, in step S35, the mixture 811 from step S32, the aqueous solution A 812, and the aqueous solution B 813 are mixed.
[0534] As a mixing method in step S35, a mixing method can be used in which the mixture 811 of step S32 and the aqueous solution B 813 are dropped into the aqueous solution A 812 placed in a reaction vessel. It is desirable to drop the mixture 811 of step S32 at a constant rate and to drop the aqueous solution B 813 appropriately to maintain the pH of the mixed solution in the reaction vessel within a predetermined range. In the mixing in step S35, it is desirable to stir the solution in the reaction vessel with a stirring blade or a stirrer, and the solution in the reaction vessel, the mixture 811 of step S32, the aqueous solution A 812, and the aqueous solution B 813 are stirred with N 2 It is desirable to remove dissolved oxygen by bubbling. In the mixing of step S35, the pH in the reaction vessel is preferably 9 or more and 11 or less, more preferably 10.0 or more and 10.5 or less. In the mixing of step S35, the temperature of the solution in the reaction vessel is preferably 40°C or more and 80°C or less, more preferably 50°C or more and 70°C or less.
[0535] Alternatively, the mixing method in step S35 may be a method of adding aqueous solution A812 and aqueous solution B813 dropwise to the mixture 811 of step S32 placed in a reaction vessel. In order to maintain the solute ion concentration and hydroxyl group concentration of aqueous solution A812 in the reaction vessel within a predetermined range, it is preferable to adjust the drop speed of aqueous solution A812 and aqueous solution B813. In the mixing in step S35, it is preferable to stir the solution in the reaction vessel with a stirring blade or a stirrer, and the solution in the reaction vessel, the mixture 811 of step S32, aqueous solution A812, and aqueous solution B813 are stirred with N 2 It is desirable to remove dissolved oxygen by bubbling. In the mixing in step S35, the temperature of the solution in the reaction vessel is preferably 40°C or higher and 80°C or lower, more preferably 50°C or higher and 70°C or lower.
[0536] Alternatively, a case where the aqueous solution A 812 is not used as the mixing method in step S35 will be described. A certain amount of the aqueous solution B 813 is added dropwise to the mixture 811 of step S32 placed in a reaction vessel. In the mixing in step S35, it is desirable to stir the solution in the reaction vessel with a stirring blade or a stirrer. The solution in the reaction vessel, the mixture 811 of step S32, and the aqueous solution B 813 are stirred with N 2 It is desirable to remove dissolved oxygen by bubbling. In the mixing in step S35, the temperature of the solution in the reaction vessel is preferably 40°C or higher and 80°C or lower, more preferably 50°C or higher and 70°C or lower.
[0537] Alternatively, as a method of mixing in step S35, a case will be described in which pure water is used in addition to the mixture 811, aqueous solution A 812, and aqueous solution B 813 of step S32. The mixture 811 and aqueous solution A 812 of step S32 are added dropwise at a constant rate to the pure water placed in a reaction vessel, and aqueous solution B 813 can be added dropwise as needed to maintain the pH of the mixed solution in the reaction vessel within a predetermined range. In the mixing in step S35, it is desirable to stir the solution in the reaction vessel with a stirring blade or a stirrer, and the solution in the reaction vessel, the mixture 811 of step S32, aqueous solution A 812, and aqueous solution B 813 are stirred with N 2 It is desirable to remove dissolved oxygen by bubbling. In the mixing of step S35, the pH in the reaction vessel is preferably 9 or more and 11 or less, more preferably 10.0 or more and 10.5 or less. In the mixing of step S35, the temperature of the solution in the reaction vessel is preferably 40°C or more and 80°C or less, more preferably 50°C or more and 70°C or less.
[0538] Next, in step S36, the solution containing the hydroxide having the transition metal M1 formed by the mixing in step S35 is filtered and then washed with water. The water used for washing is preferably pure water with a low impurity content, preferably with a resistivity of 1 MΩ cm or more, more preferably 10 MΩ cm or more, and even more preferably 15 MΩ cm or more. By using pure water with a low impurity content for washing, impurities contained in the hydroxide having the transition metal M1 can be removed, and a high-purity hydroxide having the transition metal M1 can be obtained as a reaction precursor.
[0539] Next, in step S36, the washed hydroxide containing the transition metal M1 is dried and recovered to obtain the mixture 821 of step S41.
[0540] Next, in step S42, lithium compound 803 is prepared, and in step S51, mixture 821 from step S41 and lithium compound 803 are mixed. After mixing, the mixture is recovered in step S52, and mixture 831 is obtained in step S53. Mixing can be performed by either a dry method or a wet method. For example, a ball mill, a bead mill, or the like can be used for mixing. When using a ball mill, it is preferable to use zirconia balls as the medium. Furthermore, when using a ball mill, a bead mill, or the like, it is preferable to set the peripheral speed to 100 mm / s or more and 2000 mm / s or less to suppress contamination from the media or materials. Note that step S42 is performed at a peripheral speed of 838 mm / s (rotation speed: 400 rpm, diameter of ball mill container: 40 mm).
[0541] As the lithium compound 803, for example, lithium hydroxide, lithium carbonate, lithium nitrate, or the like can be used.
[0542] It is preferable to use a high-purity material as the lithium compound 803 used in the synthesis. Specifically, the purity of the material is 4N (99.99%) or higher, preferably 4N5UP (99.995%) or higher, and more preferably 5N (99.999%) or higher. Using a high-purity material can increase the capacity and / or reliability of the secondary battery.
[0543] Next, in step S54, the mixture 831 from step S53 is heated. Heating is preferably performed at a temperature of 700° C. or higher and lower than 1100° C., more preferably 800° C. or higher and 1000° C. or lower, and even more preferably 800° C. or higher and 950° C. or lower.
[0544] The heating time can be, for example, 1 hour or more and 100 hours or less, and preferably 2 hours or more and 20 hours or less. The heating is preferably carried out in an oxygen-containing atmosphere with little water, such as oxygen or dry air (for example, a dew point of -50°C or less, more preferably a dew point of -80°C or less). In this embodiment, the heating is carried out in an atmosphere with a dew point of -93°C. The heating is carried out in a CH 4 , CO, CO 2 , and H 2 It is preferable to perform the treatment in an atmosphere in which the impurity concentrations of the above are 5 ppb (parts per billion) or less, since this can suppress impurities that may be mixed into the material.
[0545] For example, when heating at 850°C for 10 hours, the temperature increase rate is preferably 200°C / h and the flow rate of the dry atmosphere is preferably 10 L / min. The heated material can then be cooled to room temperature. For example, it is preferable that the temperature decrease time from the specified temperature to room temperature is 10 hours or more and 50 hours or less. However, cooling to room temperature in step S54 is not essential.
[0546] The crucible or sheath used in the heating step S54 is preferably made of a highly heat-resistant material such as alumina (aluminum oxide), mullite / cordierite, magnesia, or zirconia. An alumina crucible is preferable because it is a material that does not contain impurities. In this embodiment, an alumina crucible with a purity of 99.9% is preferably used. It is preferable to heat the crucible or sheath with a lid, which prevents the material from volatilizing.
[0547] Furthermore, when recovering the material after heating in step S54, it is preferable to transfer the material from the crucible to a mortar and then recover it, since this prevents impurities from being mixed into the material. Furthermore, it is also preferable for the mortar to be made of a material that does not allow impurities to be mixed in. Specifically, it is preferable to use a mortar made of alumina with a purity of 90 wt% or more, preferably 99 wt% or more.
[0548] Next, in step S55, the fired material is recovered, and in step S56, positive electrode active material 100G is obtained. Positive electrode active material 100G can be used as first material 100x shown in Embodiments 1 and 2.
[0549] [Method 2 for Manufacturing Positive Electrode Active Material] Another example of a method for manufacturing a positive electrode active material of one embodiment of the present invention will be described with reference to FIGS. 38 and 39A to 39E.
[0550] Steps S21 to S55 in FIG. 38 can be performed in the same manner as in the method shown in FIG.
[0551] Next, in step S62, an additive element X source 833 is prepared.
[0552] The additive element X source can be one or more selected from nickel, cobalt, magnesium, calcium, chlorine, fluorine, bromine, aluminum, manganese, titanium, zirconium, yttrium, vanadium, iron, chromium, niobium, lanthanum, hafnium, zinc, silicon, sulfur, phosphorus, boron, and arsenic. The additive element X source 833 in step S62 can be any one or more of an aqueous solution containing the additive element X, an alkoxide containing the additive element X, or a solid compound containing the additive element X. For example, as shown in S62a or S62b in FIGS. 39A and 39B, a solid compound containing one or more additive elements X may be prepared, crushed, and mixed to be used as the additive element X source 833 in step S62. When a solid compound containing one or more additional elements X is used, it may be mixed after being crushed, or may be mixed and crushed, or may be used as the additional element X source 833 in step S62 without being crushed.
[0553] It is preferable to use a high-purity material as the source of the additive element X used in the synthesis. Specifically, the purity of the material is 2N (99%) or higher, preferably 3N (99.9%) or higher, and more preferably 4N (99.99%) or higher. The use of a high-purity material can increase the capacity and / or reliability of the secondary battery.
[0554] When the mixing and crushing steps are performed wet, a solvent is prepared. Examples of solvents that can be used include ketones such as acetone, alcohols such as ethanol and isopropanol, ether, dioxane, acetonitrile, and N-methyl-2-pyrrolidone (NMP). It is more preferable to use an aprotic solvent that is less likely to react with lithium. In this embodiment, dehydrated acetone with a purity of 99.5% or higher is used.
[0555] Next, in step S71, the mixture 832 from step S61 is mixed with the additive element X source 833 from step S62. After mixing, the mixture is recovered in step S72, and a mixture 841 is obtained in step S73. Mixing can be performed by either a dry method or a wet method. For example, a ball mill, a bead mill, or the like can be used for mixing. When using a ball mill, it is preferable to use zirconia balls as the media. Furthermore, when using a ball mill, a bead mill, or the like, it is preferable to set the peripheral speed to 100 mm / s or more and 2000 mm / s or less in order to suppress contamination from the media or materials. Note that step S71 is performed at a peripheral speed of 838 mm / s (rotation speed 400 rpm, diameter of ball mill container 40 mm).
[0556] Next, in step S74, the mixture 841 from step S73 is heated. The heating temperature in step S74 is preferably 500°C or higher and 1100°C or lower, more preferably 500°C or higher and 1000°C or lower, even more preferably 500°C or higher and 950°C or lower, and still more preferably 500°C or higher and 900°C or lower.
[0557] Furthermore, the heating in step S74 may be performed using a roller hearth kiln. When performing heat treatment in a roller hearth kiln, the mixture 841 may be treated using a heat-resistant container with a lid.
[0558] The heating time can be, for example, 1 hour or more and 100 hours or less, and preferably 2 hours or more and 20 hours or less. The heating is preferably carried out in an oxygen-containing atmosphere with little water, such as oxygen or dry air (for example, a dew point of -50°C or less, more preferably a dew point of -80°C or less). In this embodiment, the heating is carried out in an atmosphere with a dew point of -93°C. The heating is carried out in a CH 4 , CO, CO 2 , and H 2 It is preferable to perform the treatment in an atmosphere in which the impurity concentrations of the above are 5 ppb (parts per billion) or less, since this can suppress impurities that may be mixed into the material.
[0559] For example, when heating at 850°C for 10 hours, the temperature increase rate is preferably 200°C / h and the flow rate of the dry atmosphere is preferably 10 L / min. The heated material can then be cooled to room temperature. For example, it is preferable that the temperature decrease time from the specified temperature to room temperature is 10 hours or more and 50 hours or less. However, cooling to room temperature in step S74 is not essential.
[0560] Next, in step S75, the fired material is recovered to obtain mixture 842 of step S81. Mixture 842 obtained in step S81 can be used as positive electrode active material 100. Mixture 842 obtained in step S81 can also be subjected to the steps subsequent to step S81 shown in FIG.
[0561] Next, the steps from step S81 onwards shown in Fig. 39C will be described. In step S82, an additive element X source 843 is prepared.
[0562] The additive element X added in step S82 can be selected from the additive elements X described above. The additive element X source 843 in step S82 can be any one or more of an aqueous solution containing the additive element X, an alkoxide containing the additive element X, or a solid compound containing the additive element X. For example, as shown in S82a or S82b in FIGS. 39D and 39E , a solid compound containing one or more additive elements X may be prepared, crushed, and mixed to be used as the additive element X source 843 in step S82. When a solid compound containing one or more additive elements X is used, it may be mixed after crushing, or crushed after mixing, or it may be used as the additive element X source 843 in step S82 without being crushed.
[0563] It is preferable to use a high-purity material as the source of the additive element X used in the synthesis. Specifically, the purity of the material is 2N (99%) or higher, preferably 3N (99.9%) or higher, and more preferably 4N (99.99%) or higher. The use of a high-purity material can increase the capacity and / or reliability of the secondary battery.
[0564] Next, in step S91, the mixture 842 from step S81 and the additive element X source 843 from step S82 are mixed. After mixing, the mixture is recovered in step S92, and a mixture 851 is obtained in step S93. Mixing can be performed in a dry or wet manner. For example, a ball mill, a bead mill, or the like can be used for mixing. When using a ball mill, it is preferable to use zirconia balls as the medium. Furthermore, when using a ball mill, a bead mill, or the like, it is preferable to set the peripheral speed to 100 mm / s or more and 2000 mm / s or less to suppress contamination from the media or materials. In step S91, dry mixing is performed in a ball mill using zirconia balls with a diameter of 1 mm at 150 rpm for 1 hour. Furthermore, the mixing is performed in a dry room with a dew point of -100°C to -10°C.
[0565] Next, in step S94, the mixture 851 from step S93 is heated. The heating temperature in step S94 is preferably 500°C or higher and 1130°C or lower, more preferably 500°C or higher and 1000°C or lower, even more preferably 500°C or higher and 950°C or lower, and still more preferably 500°C or higher and 900°C or lower.
[0566] The heating time can be, for example, 1 hour or more and 100 hours or less, and preferably 2 hours or more and 20 hours or less. The heating is preferably carried out in an oxygen-containing atmosphere with little water, such as oxygen or dry air (for example, a dew point of -50°C or less, more preferably a dew point of -80°C or less). In this embodiment, the heating is carried out in an atmosphere with a dew point of -93°C. The heating is carried out in a CH 4 , CO, CO 2 , and H 2 It is preferable to perform the treatment in an atmosphere in which the impurity concentrations of the above are 5 ppb (parts per billion) or less, since this can suppress impurities that may be mixed into the material.
[0567] For example, when heating at 850°C for 10 hours, the temperature increase rate is preferably 200°C / h and the flow rate of the dry atmosphere is preferably 10 L / min. The heated material can then be cooled to room temperature. For example, it is preferable that the temperature decrease time from the specified temperature to room temperature is 10 hours or more and 50 hours or less. However, cooling to room temperature in step S74 is not essential.
[0568] However, cooling to room temperature in step S94 is not essential, and cooling to a temperature higher than room temperature may be performed if there is no problem in carrying out the subsequent steps.
[0569] Next, in step S95, the fired material is recovered, and positive electrode active material 100H is obtained in step S101. Positive electrode active material 100H can be used as first material 100x shown in Embodiments 1 and 2.
[0570] [Method 3 for Manufacturing Positive Electrode Active Material] Another example of a method for manufacturing a positive electrode active material of one embodiment of the present invention will be described with reference to FIGS.
[0571] 40, a transition metal M1 source 800 is prepared. In this embodiment, a case will be described in which three types of transition metal M1 sources 800, namely, a nickel source 800a, a cobalt source 800b, and a manganese source 800c, are used.
[0572] The nickel-containing aqueous solution of the nickel source 800a may be a nickel sulfate aqueous solution or a nickel nitrate aqueous solution, etc. The cobalt-containing aqueous solution of the cobalt source 800b may be a cobalt sulfate aqueous solution or a cobalt nitrate aqueous solution, etc. The manganese-containing aqueous solution of the manganese source 800c may be a manganese sulfate aqueous solution or a manganese nitrate aqueous solution, etc.
[0573] It is preferable to use a high-purity material as the transition metal M1 source 800 used in the synthesis. Specifically, when using an aqueous solution containing the transition metal M1, the purity of the solute material when preparing the aqueous solution is 2N (99%) or higher, preferably 3N (99.9%) or higher, and more preferably 4N (99.99%) or higher. The water is preferably pure water with a low impurity content, preferably with a resistivity of 1 MΩ cm or higher, more preferably 10 MΩ cm or higher, and even more preferably 15 MΩ cm or higher. The use of a high-purity material can increase the capacity and / or reliability of the secondary battery.
[0574] When using metals capable of forming a layered rock salt type composite oxide, it is preferable to set the mixing ratio of cobalt, manganese, and nickel within a range that allows a layered rock salt type crystal structure to be formed.
[0575] Next, in step S31, the nickel source 800a, the cobalt source 800b, and the manganese source 800c are mixed together to obtain a mixture 811 in step S32.
[0576] Next, an aqueous solution A 812 is prepared in step S33, and an aqueous solution B 813 is prepared in step S34.
[0577] As the aqueous solution A812, one or a mixture of a solution containing at least one of chelating agents such as glycine, oxine, 1-nitroso-2-naphthol, or 2-mercaptobenzothiazole, or ammonia water can be used.
[0578] As the aqueous solution B813, any one of an aqueous solution of sodium hydroxide, an aqueous solution of potassium hydroxide, and an aqueous solution of lithium hydroxide, or a mixture of two or more thereof can be used.
[0579] Next, in step S35, the mixture 811 from step S32, the aqueous solution A 812, and the aqueous solution B 813 are mixed.
[0580] Steps S35 to S55 in FIG. 40 can be performed in the same manner as in the method shown in FIG.
[0581] Next, in steps S63 and S64, a magnesium source 834 and a fluorine source 835 are prepared as sources of the additional element X. Subsequently, in step S65, the magnesium source 834 and the fluorine source 835 are crushed and mixed to obtain a mixture 836 in step S66.
[0582] The magnesium source 834 may be, for example, magnesium fluoride, magnesium oxide, magnesium hydroxide, magnesium carbonate, or the like.
[0583] The fluorine source 835 may be, for example, lithium fluoride (LiF), magnesium fluoride (MgF 2 ), aluminum fluoride (AlF 3 ), titanium fluoride (TiF 4 ), cobalt fluoride (CoF 2 , CoF 3 ), nickel fluoride (NiF 2 ), zirconium fluoride (ZrF 4 ), vanadium fluoride (VF 5 ), manganese fluoride, iron fluoride, chromium fluoride, niobium fluoride, zinc fluoride (ZnF 2 ), calcium fluoride (CaF 2 ) Sodium fluoride (NaF), potassium fluoride (KF), barium fluoride (BaF 2 ), cerium fluoride (CeF 2 ), lanthanum fluoride (LaF 3 ) Sodium aluminum hexafluoride (Na 3 AlF 6 The fluorine source is not limited to a solid, and may be, for example, fluorine (F 2 ), fluorocarbon, sulfur fluoride, oxygen fluoride (OF 2 , O 2 F 2 , O 3 F 2 , O 4 F 2 , O 2 Fluorine sources such as lithium fluoride (F) may be used and mixed into the atmosphere during the heating step described below. A mixture of multiple fluorine sources may also be used. Among these, lithium fluoride is preferred because it has a relatively low melting point of 848°C and is easily melted during the annealing step described below.
[0584] In this embodiment, lithium fluoride (LiF) is prepared as the fluorine source, and magnesium fluoride (MgF) is prepared as the fluorine source and magnesium source. 2 Lithium fluoride (LiF) and magnesium fluoride (MgF) 2 is LiF:MgF 2 Mixing lithium fluoride (LiF) and magnesium fluoride (MgF) in a molar ratio of about 65:35 results in the greatest effect of lowering the melting point. On the other hand, if the amount of lithium fluoride is too high, there is a concern that the lithium content will be excessive, which may deteriorate the cycle characteristics. Therefore, a mixture of lithium fluoride (LiF) and magnesium fluoride (MgF) 2 The molar ratio of LiF:MgF 2 =x:1 (0≦x≦1.9), and LiF:MgF 2 =x:1 (0.1≦x≦0.5) is more preferable, and LiF:MgF 2 = x: 1 (x = near 0.33) is more preferable. In this specification, "near" refers to a value that is greater than 0.9 times and smaller than 1.1 times the value.
[0585] Furthermore, if the crushing and mixing process in step S65 is performed wet, a solvent is prepared. Examples of solvents that can be used include ketones such as acetone, alcohols such as ethanol and isopropanol, ether, dioxane, acetonitrile, and N-methyl-2-pyrrolidone (NMP). It is more preferable to use an aprotic solvent that is less likely to react with lithium. In this embodiment, dehydrated acetone with a purity of 99.5% or higher is used.
[0586] It is preferable to use high-purity materials as the magnesium source and fluorine source used in the synthesis. Specifically, the purity of the materials is 4N (99.99%) or higher, preferably 4N5UP (99.995%) or higher, and more preferably 5N (99.999%) or higher. The use of high-purity materials can increase the capacity and / or reliability of the secondary battery.
[0587] Next, in step S71, the mixture 832 from step S61 and the mixture 836 from step S66 are mixed. After mixing, the mixture is recovered in step S72, and a mixture 841 is obtained in step S73. Mixing can be performed by either a dry method or a wet method. For example, a ball mill, a bead mill, or the like can be used for mixing. When using a ball mill, it is preferable to use zirconia balls as the media. Furthermore, when using a ball mill, a bead mill, or the like, it is preferable to set the peripheral speed to 100 mm / s or more and 2000 mm / s or less in order to suppress contamination from the media or materials. Note that step S71 is performed at a peripheral speed of 838 mm / s (rotation speed 400 rpm, diameter of ball mill container 40 mm).
[0588] Next, in step S74, the mixture 841 from step S73 is heated. The heating temperature in step S74 is preferably 500°C or higher and 1100°C or lower, more preferably 500°C or higher and 1000°C or lower, even more preferably 500°C or higher and 950°C or lower, and still more preferably 500°C or higher and 900°C or lower.
[0589] Furthermore, the heating in step S74 may be performed using a roller hearth kiln. When performing heat treatment in a roller hearth kiln, the mixture 841 may be treated using a heat-resistant container with a lid.
[0590] The heating time can be, for example, 1 hour or more and 100 hours or less, and preferably 2 hours or more and 20 hours or less. The heating is preferably carried out in an oxygen-containing atmosphere with little water, such as oxygen or dry air (for example, a dew point of -50°C or less, more preferably a dew point of -80°C or less). In this embodiment, the heating is carried out in an atmosphere with a dew point of -93°C. The heating is carried out in a CH 4 , CO, CO 2 , and H 2 It is preferable to perform the treatment in an atmosphere in which the impurity concentrations of the above are 5 ppb (parts per billion) or less, since this can suppress impurities that may be mixed into the material.
[0591] For example, when heating at 850°C for 10 hours, the temperature increase rate is preferably 200°C / h and the flow rate of the dry atmosphere is preferably 10 L / min. The heated material can then be cooled to room temperature. For example, it is preferable that the temperature decrease time from the specified temperature to room temperature is 10 hours or more and 50 hours or less. However, cooling to room temperature in step S74 is not essential.
[0592] Next, in step S75, the fired material is recovered to obtain mixture 842 of step S81. Mixture 842 obtained in step S81 can be used as positive electrode active material 100. Mixture 842 obtained in step S81 can also be subjected to the steps subsequent to step S81 shown in FIG.
[0593] Next, the steps from step S81 onwards shown in Fig. 41 will be described. In steps S83 and S84, a nickel source 845 and an aluminum source 846 are prepared as sources of additional element X. In steps S85 and S86, the nickel source 845 and the aluminum source 846 are crushed, respectively, and mixed in step S87 to obtain a mixture 847 in step S88.
[0594] As the nickel source, nickel oxide, nickel hydroxide, etc. can be used.
[0595] As the aluminum source, aluminum oxide, aluminum hydroxide, etc. can be used.
[0596] It is preferable to use high-purity materials as the nickel source and aluminum source used in the synthesis. Specifically, the purity of the materials is 4N (99.99%) or higher, preferably 4N5UP (99.995%) or higher, and more preferably 5N (99.999%) or higher. The use of high-purity materials can increase the capacity and / or reliability of the secondary battery.
[0597] Next, in step S91, the mixture 842 from step S81 and the mixture 847 from step S88 are mixed. After mixing, the mixture is recovered in step S92, and mixture 851 is obtained in step S93. Mixing can be performed in a dry or wet manner. For example, a ball mill, a bead mill, or the like can be used for mixing. When using a ball mill, it is preferable to use zirconia balls as the medium. Furthermore, when using a ball mill, a bead mill, or the like, it is preferable to set the peripheral speed to 100 mm / s or more and 2000 mm / s or less to suppress contamination from the media or materials. In step S91, dry mixing is performed in a ball mill using zirconia balls with a diameter of 1 mm at 150 rpm for 1 hour. Furthermore, the mixing is performed in a dry room with a dew point of -100°C to -10°C.
[0598] Next, in step S94, the mixture 851 from step S93 is heated. The heating temperature in step S94 is preferably 500°C or higher and 1130°C or lower, more preferably 500°C or higher and 1000°C or lower, even more preferably 500°C or higher and 950°C or lower, and still more preferably 500°C or higher and 900°C or lower.
[0599] The heating time can be, for example, 1 hour or more and 100 hours or less, and preferably 2 hours or more and 20 hours or less. The heating is preferably carried out in an oxygen-containing atmosphere with little water, such as oxygen or dry air (for example, a dew point of -50°C or less, more preferably a dew point of -80°C or less). In this embodiment, the heating is carried out in an atmosphere with a dew point of -93°C. The heating is carried out in a CH 4 , CO, CO 2 , and H 2 It is preferable to perform the treatment in an atmosphere in which the impurity concentrations of the above are 5 ppb (parts per billion) or less, since this can suppress impurities that may be mixed into the material.
[0600] For example, when heating at 850°C for 10 hours, the temperature increase rate is preferably 200°C / h and the flow rate of the dry atmosphere is preferably 10 L / min. The heated material can then be cooled to room temperature. For example, it is preferable that the temperature decrease time from the specified temperature to room temperature is 10 hours or more and 50 hours or less. However, cooling to room temperature in step S74 is not essential.
[0601] Next, in step S95, the fired material is recovered, and in step S101, positive electrode active material 100J is obtained. Positive electrode active material 100J can be used as first material 100x shown in Embodiments 1 and 2.
[0602] [Method 4 for Manufacturing Positive Electrode Active Material] Another example of a method for manufacturing a positive electrode active material of one embodiment of the present invention will be described with reference to FIGS.
[0603] In step S21 of FIG. 42, a transition metal M1 source 800 is prepared, and in step S22, an additional element X source 801 is prepared.
[0604] The transition metal M1 may be, for example, at least one of manganese, cobalt, and nickel. For example, the transition metal M1 may be composed of only cobalt, only nickel, two metals, cobalt and manganese, two metals, cobalt and nickel, or three metals, cobalt, manganese, and nickel. The source of the transition metal M1 is prepared as an aqueous solution containing the transition metal M1.
[0605] As the transition metal M1 source 800, an aqueous solution containing cobalt such as an aqueous cobalt sulfate solution or an aqueous cobalt nitrate solution can be used, an aqueous solution containing nickel such as an aqueous nickel sulfate solution or an aqueous nickel nitrate solution can be used, and an aqueous solution containing manganese such as an aqueous manganese sulfate solution or an aqueous manganese nitrate solution can be used.
[0606] It is preferable to use a high-purity material as the transition metal M1 source 800 used in the synthesis. Specifically, when using an aqueous solution containing the transition metal M1, the purity of the solute material when preparing the aqueous solution is 2N (99%) or higher, preferably 3N (99.9%) or higher, and more preferably 4N (99.99%) or higher. The water is preferably pure water with a low impurity content, preferably with a resistivity of 1 MΩ cm or higher, more preferably 10 MΩ cm or higher, and even more preferably 15 MΩ cm or higher. The use of a high-purity material can increase the capacity and / or reliability of the secondary battery.
[0607] The additive element X source 801 can be one or more selected from nickel, cobalt, magnesium, calcium, chlorine, fluorine, bromine, aluminum, manganese, titanium, zirconium, yttrium, vanadium, iron, chromium, niobium, lanthanum, hafnium, zinc, silicon, sulfur, phosphorus, boron, and arsenic. The additive element X source 801 can be any one or more of an aqueous solution containing the additive element X, an alkoxide containing the additive element X, or a solid compound containing the additive element X. The additive element X source 801 in step S22 is preferably prepared as an aqueous solution containing the additive element X.
[0608] It is preferable to use a high-purity material as the additive element X source 801 used in the synthesis. Specifically, the purity of the material is 2N (99%) or higher, preferably 3N (99.9%) or higher, and more preferably 4N (99.99%) or higher. By using a high-purity material, it is possible to increase the capacity and / or reliability of the secondary battery.
[0609] Next, in step S31, the transition metal M1 source and the additive element X source are mixed together to obtain a mixture 811 in step S32.
[0610] Next, an aqueous solution A 812 is prepared in step S33, and an aqueous solution B 813 is prepared in step S34.
[0611] As the aqueous solution A812, one or a mixture of a solution containing at least one of chelating agents such as glycine, oxine, 1-nitroso-2-naphthol, or 2-mercaptobenzothiazole, or ammonia water can be used.
[0612] As the aqueous solution B813, any one of an aqueous solution of sodium hydroxide, an aqueous solution of potassium hydroxide, and an aqueous solution of lithium hydroxide, or a mixture of two or more thereof can be used.
[0613] Next, in step S35, the mixture 811 from step S32, the aqueous solution A 812, and the aqueous solution B 813 are mixed.
[0614] Steps S35 to S54 in FIG. 42 can be performed in the same manner as in the method shown in FIG.
[0615] Next, in step S55, the fired material is recovered, and in step S56, positive electrode active material 100K is obtained. Positive electrode active material 100K can be used as first material 100x shown in Embodiments 1 and 2.
[0616] [Method 5 for Manufacturing Positive Electrode Active Material] Another example of a method for manufacturing a positive electrode active material of one embodiment of the present invention will be described with reference to FIGS.
[0617] Steps S21 to S41 in FIG. 43 can be performed in the same manner as in the method shown in FIG.
[0618] Next, in step S42, a lithium compound 803 is prepared, and in step S43, an additional element X source 801 is prepared. In step S51, the mixture 821 of step S41, the lithium compound 803, and the additional element X source 801 are mixed.
[0619] Steps S51 to S54 in FIG. 43 can be performed in the same manner as in the method shown in FIG.
[0620] Next, in step S55, the fired material is recovered, and in step S56, positive electrode active material 100L is obtained. Positive electrode active material 100L can be used as first material 100x shown in Embodiments 1 and 2.
[0621] [Method 6 for Manufacturing Positive Electrode Active Material] Another example of a method for manufacturing a positive electrode active material of one embodiment of the present invention will be described with reference to FIGS.
[0622] Steps S21 to S74 in FIG. 44 can be performed in the same manner as in the method shown in FIG.
[0623] Next, in step S75, the fired material is recovered, and in step S76, a positive electrode active material 100M is obtained. The positive electrode active material 100M can be used as the first material 100x shown in Embodiments 1 and 2.
[0624] [Method 7 for Manufacturing Positive Electrode Active Material] Another example of a method for manufacturing a positive electrode active material of one embodiment of the present invention will be described with reference to FIGS.
[0625] Steps S21 to S41 in Fig. 45 can be performed in the same manner as the method shown in Fig. 42. Furthermore, steps S42 to S54 in Fig. 45 can be performed in the same manner as the method shown in Fig. 43.
[0626] Next, in step S55, the fired material is recovered, and in step S56, positive electrode active material 100N is obtained. Positive electrode active material 100N can be used as first material 100x shown in Embodiments 1 and 2.
[0627] [Method 8 for Manufacturing Positive Electrode Active Material] Another example of a method for manufacturing a positive electrode active material of one embodiment of the present invention will be described with reference to FIGS.
[0628] Steps S21 to S54 in Fig. 46 can be performed in the same manner as the method shown in Fig. 43. Furthermore, steps S55 to S74 in Fig. 46 can be performed in the same manner as the method shown in Fig. 38.
[0629] Next, in step S75, the fired material is recovered, and in step S76, positive electrode active material 100P is obtained. Positive electrode active material 100P can be used as first material 100x shown in Embodiments 1 and 2.
[0630] [Method 9 for Manufacturing Positive Electrode Active Material] Another example of a method for manufacturing a positive electrode active material of one embodiment of the present invention will be described with reference to FIGS.
[0631] Steps S21 to S54 in Fig. 47 can be performed in the same manner as the method shown in Fig. 45. Also, steps S55 to S74 in Fig. 47 can be performed in the same manner as the method shown in Fig. 38.
[0632] Next, in step S75, the fired material is recovered, and in step S76, positive electrode active material 100Q is obtained. Positive electrode active material 100Q can be used as first material 100x shown in Embodiments 1 and 2.
[0633] 38 to 47, by separating the step of introducing the transition metal M1 from the multiple steps of introducing the additional element X, it may be possible to change the depth profile of each element. For example, the concentration of the additional element can be increased near the surface compared to the interior of the particle. Furthermore, using the number of atoms of the transition metal M1 as a reference, the ratio of the number of atoms of the additional element to this reference can be made higher near the surface than in the interior.
[0634] The positive electrode active material 100 is a composite oxide (LiMO) containing lithium, a transition metal M1, and oxygen. 2 However, the positive electrode active material of one embodiment of the present invention may be expressed as LiMO 2 The composition is not strictly limited to Li:M1:O=1:1:2, so long as it has a crystalline structure of a lithium composite oxide represented by the formula:
[0635] In one embodiment of the present invention, a high-purity material is used as the transition metal M1 source during synthesis, and the cathode active material is prepared through a process with minimal impurity contamination during synthesis. Furthermore, by using a preparation method in which the transition metal M1 source and impurity contamination during synthesis are thoroughly eliminated and a desired additive element (additive element X, additive element X1, or additive element X2) is controlled and introduced into the cathode active material, a cathode active material can be obtained in which regions with low impurity concentrations and regions with the additive element introduced are controlled. The cathode active material described in this embodiment is a material with high crystallinity. Furthermore, the cathode active material obtained by the method for preparing a cathode active material according to one embodiment of the present invention can increase the capacity and / or reliability of a secondary battery.
[0636] [Structure of Positive Electrode Active Material] A positive electrode active material of one embodiment of the present invention will be described with reference to FIGS. 48A to 49C.
[0637] FIG. 48A shows a cross-sectional view of positive electrode active material 100. Positive electrode active material 100 has a plurality of primary particles 101. At least some of the plurality of primary particles 101 are fixed together to form secondary particles 102. FIG. 48B shows an enlarged view of secondary particles 102. Positive electrode active material 100 may have voids 105. Note that the shapes of primary particles 101 and secondary particles 102 shown in FIGS. 48A and 48B are merely examples and are not limited to these.
[0638] In this specification, a primary particle is the smallest unit that can be recognized as a solid with clear boundaries in a microscopic image such as an SEM image, a TEM image, or an STEM image. A secondary particle is a particle formed by sintering, bonding, or agglomeration of multiple primary particles. The bonding force acting between the multiple primary particles does not matter. It may be a covalent bond, an ionic bond, a hydrophobic interaction, a van der Waals force, or other intermolecular interaction, or multiple bonding forces may be acting. Furthermore, when simply referring to particles, this includes primary particles and secondary particles.
[0639] <Contained Elements> The positive electrode active material 100 contains lithium, a transition metal M1, oxygen, and an additive element.
[0640] The positive electrode active material 100 is LiMO 2However, the positive electrode active material of one embodiment of the present invention is LiMO 2 The composition is not strictly limited to Li:M1:O=1:1:2, so long as it has a crystalline structure of a lithium composite oxide represented by the formula:
[0641] The transition metal M1 contained in the positive electrode active material 100 is preferably a metal capable of forming a layered rock-salt composite oxide belonging to the space group R-3m with lithium. For example, at least one of manganese, cobalt, and nickel can be used. That is, the transition metal contained in the positive electrode active material 100 may be cobalt alone, nickel alone, a combination of cobalt and manganese, or a combination of cobalt and nickel, or three of cobalt, manganese, and nickel. That is, the positive electrode active material 100 may contain a composite oxide containing lithium and the transition metal M1, such as lithium cobalt oxide, lithium nickel oxide, lithium cobalt oxide in which some of the cobalt is substituted with manganese, lithium cobalt oxide in which some of the cobalt is substituted with nickel, or nickel-manganese-lithium cobalt oxide.
[0642] In particular, when cobalt is used as the transition metal M1 in the positive electrode active material 100 at 75 atomic % or more, preferably at 90 atomic % or more, and more preferably at 95 atomic % or more, it has many advantages such as being relatively easy to synthesize and handle, and having excellent cycle characteristics.
[0643] On the other hand, when nickel is used as the transition metal M1 in the positive electrode active material 100 at 33 atomic % or more, preferably at 60 atomic % or more, and more preferably at 80 atomic % or more, the raw material may be cheaper than when a large amount of cobalt is used, and the charge / discharge capacity per weight may be increased, which is preferable.
[0644] Furthermore, the inclusion of nickel as a transition metal M1 along with cobalt may suppress the shift in the layered structure consisting of octahedra of cobalt and oxygen. This is preferable because the crystal structure may become more stable, particularly in the charged state at high temperatures. This is because nickel is thought to easily diffuse deep into the lithium cobalt oxide, and while present at the cobalt site during discharge, it may be located at the lithium site through cation mixing during charge. The nickel present at the lithium site during charge is thought to function as a pillar supporting the layered structure consisting of octahedra of cobalt and oxygen, contributing to the stabilization of the crystal structure.
[0645] The transition metal M1 does not necessarily have to contain manganese, nickel, or cobalt.
[0646] The additive element is preferably at least one of magnesium, fluorine, aluminum, titanium, zirconium, yttrium, vanadium, iron, chromium, niobium, lanthanum, hafnium, zinc, silicon, sulfur, phosphorus, boron, and arsenic.
[0647] In particular, by adding phosphorus to the positive electrode active material 100, the continuous charge durability can be improved, which is preferable since it allows for a highly safe secondary battery.
[0648] Furthermore, since manganese, titanium, vanadium, and chromium are materials that are stable and likely to assume a tetravalent state, using them as the transition metal M1 of the positive electrode active material 100 may increase their contribution to structural stability.
[0649] As will be described later, these added elements may further stabilize the crystal structure of the positive electrode active material 100. That is, the positive electrode active material 100 may include lithium cobalt oxide to which magnesium and fluorine have been added, lithium nickel-cobalt oxide to which magnesium and fluorine have been added, lithium cobalt-aluminate to which magnesium and fluorine have been added, nickel-cobalt-lithium aluminum oxide, nickel-cobalt-lithium aluminum oxide to which magnesium and fluorine have been added, lithium nickel-manganese-cobalt oxide to which magnesium and fluorine have been added, etc. In this specification and the like, the added element may also be referred to as a mixture, a part of a raw material, an impurity, etc.
[0650] The additive element in the positive electrode active material 100 is LiMO 2 It is preferable that the amount of the compound added is such that the crystallinity of the composite oxide represented by the formula (1) is not significantly changed. For example, it is preferable that the amount is such that the Jahn-Teller effect is not exhibited.
[0651] The additive elements do not necessarily have to include magnesium, fluorine, aluminum, titanium, zirconium, yttrium, vanadium, iron, chromium, niobium, lanthanum, hafnium, zinc, silicon, sulfur, phosphorus, boron, and arsenic.
[0652] <Element Distribution> It is preferable that at least one of the added elements in the positive electrode active material 100 has a concentration gradient.
[0653] For example, it is preferable that primary particle 101 has surface layer portion 101a and interior portion 101b, and that surface layer portion 101a has a higher concentration of the additive element than interior portion 101b. In the cross-sectional views of the positive electrode active material shown in Figures 48A and 48B, the concentration of the additive element in primary particle 101 is shown by a gradation. A darker gradation, i.e., closer to black, means that the concentration of the additive element is high, and a lighter gradation, i.e., closer to white, means that the concentration of the additive element is low.
[0654] Furthermore, the concentration of the additive element at the interface 103 between the primary particles and in the vicinity of the interface 103 is preferably higher than that in the interior 101b of the primary particle 101. In this specification and the like, the vicinity of the interface 103 refers to a region extending from the interface 103 to a distance of about 10 nm.
[0655] Fig. 49A shows an example of the concentration distribution of the added element between dashed dotted lines A and B in positive electrode active material 100 shown in Fig. 48B. In Fig. 49A, the horizontal axis represents the distance between dashed dotted lines A and B in Fig. 48B, and the vertical axis represents the added element concentration.
[0656] Compared to the single particle 101, the interface 103 and the vicinity of the interface 103 have a region where the concentration of the additional element is high. Note that the shape of the concentration distribution of the additional element is not limited to the shape shown in FIG.
[0657] Furthermore, when a plurality of additive elements are contained, it is preferable that the peak positions of the concentrations of the additive elements differ depending on the additive element.
[0658] For example, as shown in FIGS. 48A, 48B, and 49B, examples of the additive element that preferably has a concentration gradient that increases from the interior 101b toward the surface include magnesium, fluorine, and titanium.
[0659] As shown in FIG. 49C , it is preferable that some other additive elements have a concentration peak in the positive electrode active material 100 in a region closer to the interior 101b than the additive elements distributed as shown in FIG. 49B . An example of an additive element for which such a distribution is preferable is aluminum. The concentration peak may be present in the surface layer portion or deeper than the surface layer portion. For example, it is preferable that the concentration peak be present in a region 5 nm to 30 nm from the surface.
[0660] 49B, it is preferable that some of the added elements, for example, magnesium, have a concentration gradient that increases from the interior 101b toward the surface, and in addition, it is preferable that the added elements are thinly distributed throughout the primary particle 101. For example, it is preferable that the magnesium concentration in the surface layer 101a measured by XPS or the like is higher than the average magnesium concentration throughout the particle measured by ICP-MS or the like.
[0661] Furthermore, when the positive electrode active material 100 of one embodiment of the present invention contains an element other than cobalt, for example, one or more metals selected from nickel, aluminum, manganese, iron, and chromium, the concentration of the metal in the near-surface region of the primary particle 101 is preferably higher than the average concentration of the entire particle. For example, the concentration of the element other than cobalt in the surface layer portion 101 a measured by XPS or the like is preferably higher than the average concentration of the element in the entire particle measured by ICP-MS or the like.
[0662] Unlike the interior of the crystal, the particle surface is in a state where bonds are broken, and since lithium is released from the surface during charging, the surface is a portion where the lithium concentration is likely to be lower than the interior 101b. Therefore, this portion is prone to becoming unstable and the crystal structure is likely to collapse. If the concentration of the additive element in the surface layer 101a is high, changes in the crystal structure can be more effectively suppressed. Furthermore, if the concentration of the additive element in the surface layer 101a is high, it can be expected that the corrosion resistance to hydrofluoric acid produced by decomposition of the electrolyte will be improved.
[0663] As described above, the surface layer portion 101a of the positive electrode active material 100 of one embodiment of the present invention preferably has a higher concentration of the additive element than the inner portion 101b and a different composition from the inner portion 101b. Furthermore, the composition preferably has a stable crystal structure at room temperature (25°C). Therefore, the surface layer portion 101a may have a different crystal structure from the inner portion 101b. For example, at least a part of the surface layer portion 101a of the positive electrode active material 100 of one embodiment of the present invention may have a rock salt crystal structure. Furthermore, when the surface layer portion 101a and the inner portion 101b have different crystal structures, it is preferable that the crystal orientations of the surface layer portion 101a and the inner portion 101b approximately match.
[0664] However, if the surface layer 101a consists only of an additive element and oxygen, for example, only MgO, or only a structure in which MgO and CoO(II) are solid-solved, it becomes difficult to insert and extract lithium. Therefore, the surface layer 101a must contain at least a transition metal M1, and in a discharged state, it must also contain lithium, providing a path for lithium insertion and extraction. Furthermore, it is preferable that the concentration of the transition metal M1 be higher than that of each additive element.
[0665] Note that the positive electrode active material 100 of one embodiment of the present invention is not limited thereto, and may contain an additional element that does not have a concentration gradient.
[0666] It is preferable that the transition metal M1, particularly cobalt and nickel, be uniformly dissolved in the entire positive electrode active material 100 as a solid solution.
[0667] A part of the transition metal M1 contained in the positive electrode active material 100, for example, manganese, may have a concentration gradient that increases from the interior 101b toward the surface.
[0668] The distribution of the additive elements described above can reduce deterioration of the positive electrode active material 100 even after charge and discharge. That is, deterioration of the secondary battery can be suppressed. Furthermore, a highly safe secondary battery can be obtained.
[0669] Generally, as a secondary battery is repeatedly charged and discharged, side reactions such as the elution of transition metals M1, such as cobalt and manganese, from the positive electrode active material of the secondary battery into the electrolyte, the desorption of oxygen, and the instability of the crystal structure may occur, resulting in the deterioration of the positive electrode active material. The deterioration of the positive electrode active material may also lead to the deterioration of the secondary battery, such as a decrease in the capacity of the secondary battery. In this specification and the like, chemical and structural changes in the positive electrode active material, such as the elution of the transition metal M1 of the positive electrode active material ...
Claims
1. A method for producing a positive electrode active material having a first material and a second material, comprising the steps of: the first material is produced through a step of performing a first heating process on a first composite oxide containing cobalt, a step of mixing the first composite oxide with a magnesium source and a fluorine source, followed by a second heating process to produce a second composite oxide, and a step of mixing the second composite oxide with an aluminum source and a nickel source, followed by a third heating process; The temperature of the second heating is higher than the temperature of the first heating, a first step of covering at least a portion of a surface of the first material with the second material to form a composite; a second step of subjecting the composite to a fourth heat; the first material comprises lithium cobalt oxide having magnesium, fluorine, aluminum, and nickel; The second material is LiM2PO 4 (M2 is one or more selected from Fe, Ni, Co, and Mn), The fourth heating step is performed in an atmosphere containing oxygen.
2. A method for producing a positive electrode active material having a first material and a second material, comprising the steps of: the first material is produced through a step of performing a first heating process on a first composite oxide containing cobalt, a step of mixing the first composite oxide with a magnesium source and a fluorine source, followed by a second heating process to produce a second composite oxide, and a step of mixing the second composite oxide with an aluminum source and a nickel source, followed by a third heating process; The temperature of the second heating is higher than the temperature of the first heating, a first step of covering at least a portion of a surface of the first material with the second material to form a composite; a second step of subjecting the composite to a fourth heat; the first material comprises lithium cobalt oxide having magnesium, fluorine, aluminum, and nickel; the second material comprises aluminum oxide; The fourth heating step is performed in an atmosphere containing oxygen.
3. In claim 1 or 2, The fourth heating is performed at a temperature of 450° C. or higher and 800° C. or lower.