Secondary battery, power storage system, vehicle, and positive electrode production method
Patent Information
- Application Number
- JP2022563254
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2020-12-16
- Filing Date
- 2021-11-09
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2041-11-09
AI Technical Summary
Current secondary battery positive electrode active materials face challenges in stability and reliability, particularly at high potentials and temperatures, leading to deterioration during charge/discharge cycles, which affects their capacity and longevity.
Incorporating a composite compound with crystallinity that functions as both a binder and electrolyte, preventing direct contact between the active material and organic electrolyte, and using materials like magnesium and cobalt oxides with surface roughness less than 3 nm, along with conductive materials like carbon black or graphene, to enhance stability and ionic conductivity.
The solution results in a secondary battery with improved charge/discharge cycle characteristics, increased discharge capacity, and enhanced stability, reducing material degradation and maintaining performance over repeated cycles.
Abstract
Description
Secondary battery, power storage system, vehicle, and method for manufacturing positive electrode
[0001] The present invention relates to a secondary battery having a positive electrode, a power storage system having a secondary battery, a vehicle, etc., and a method for manufacturing the secondary battery and the positive electrode.
[0002] The present invention also relates to a process, a machine, manufacture, or a composition of matter.One embodiment of the present invention relates to a semiconductor device, a display device, a light-emitting device, a power storage device, a lighting device, an electronic device, or a manufacturing method thereof.
[0003] In this specification, the term "semiconductor device" refers to any device that can function by utilizing semiconductor characteristics, and electro-optical devices, semiconductor circuits, and electronic devices are all included in the category of semiconductor devices.
[0004] In this specification, the term "electronic device" refers to devices in general that have a positive electrode active material, a secondary battery, a power storage device, or a power storage system, and information terminal devices and the like that have a secondary battery are included in the electronic device.
[0005] In this specification, the term "power storage device" refers to elements and devices in general that have a power storage function, and includes, for example, power storage devices such as lithium ion secondary batteries (also simply referred to as secondary batteries), lithium ion capacitors, and electric double layer capacitors.
[0006] In recent years, various types of power storage devices, such as lithium-ion secondary batteries and lithium-ion capacitors, have been actively developed. Demand for high-power, high-energy-density lithium-ion secondary batteries has rapidly expanded in conjunction with the development of the semiconductor industry, and they are now essential to the modern information society as a rechargeable energy source, and are used in portable information terminals such as mobile phones, smartphones, and notebook computers, portable music players, digital cameras, medical devices, home energy storage systems, industrial energy storage systems, and clean-energy vehicles such as hybrid vehicles (HVs), electric vehicles (EVs), and plug-in hybrid vehicles (PHVs).
[0007] Composite oxides such as lithium cobalt oxide and lithium nickel-cobalt-manganese oxide, which have a layered rock salt structure, are widely used as positive electrode active materials for lithium-ion secondary batteries. These composite oxides offer useful properties, such as high capacity and high discharge voltage. To achieve high capacity, the positive electrode active material must be exposed to a high potential during charging. Under such high potential conditions, significant lithium desorption can reduce the stability of the composite oxide's crystalline structure, resulting in significant degradation during charge-discharge cycles. Against this background, efforts to improve the positive electrode active materials of secondary batteries have been actively pursued in order to achieve high capacity and high stability (see, for example, Patent Documents 1 to 3).
[0008] JP 2018-088400 A, WO 2018 / 203168 Pamphlet, JP 2020-140954 A
[0009] Toyoki Okumura et al, “Correlation of lithium ion distribution and X-ray absorption near-edge structure in O3-and O2-lithium cobalt oxides from first-principle calculation”, Journal of Materials Chemistry, 2012, 22, p. 17340-17348 Motohashi, T. et al, “Electronic phase diagram of the layered cobalt oxide system LixCoO▲2▼(0.0≦x≦1.0)”, Physical Review B, 80 (16), 2009, 165114 Zhaohui Chen et al, “Staging Phase Transitions in LixCoO▲2▼”, Journal of The Electrochemical Society, 2002, 149(12) A1604-A1609W. E. Counts et al, Journal of the American Ceramic Society, 1953, 36[1] 12-17. Belsky, A. et al. , “New developments in the Inorganic Crystal Structure Database (ICSD): accessibility in support of materials research and design”, Acta Crystal. , 2002, B58 364-369.
[0010] Although the positive electrode active materials have been actively improved as described in the above Patent Documents 1 to 3, there is still room for improvement in the positive electrode active materials in view of various aspects such as reliability and safety of secondary batteries.
[0011] Therefore, an object of one embodiment of the present invention is to provide a highly reliable or safe secondary battery and a manufacturing method thereof, or to provide a secondary battery with excellent charge-discharge cycle characteristics and a manufacturing method thereof, or to provide a secondary battery with a large discharge capacity and a manufacturing method thereof.
[0012] In order to realize the above secondary battery, an object of one embodiment of the present invention is to provide a positive electrode or a negative electrode that is stable in a high potential state and / or a high temperature state and a manufacturing method thereof.
[0013] In order to realize the above-described positive electrode or negative electrode, an object is to provide a positive electrode active material or negative electrode active material whose crystal structure is not easily deformed even after repeated charge and discharge, and a manufacturing method thereof. Alternatively, an object is to provide a positive electrode active material or negative electrode active material with excellent charge and discharge cycle characteristics, and a manufacturing method thereof. Alternatively, an object is to provide a positive electrode active material or negative electrode active material with a large discharge capacity, and a manufacturing method thereof.
[0014] Note that the description of these problems does not preclude the existence of other problems. Note that one embodiment of the present invention does not necessarily solve all of these problems. Note that problems other than these can be extracted from the description in the specification, drawings, and claims.
[0015] The present inventors have discovered a configuration in which a positive electrode or a negative electrode in a secondary battery is stable under high potential conditions and / or high temperatures, and the positive electrode or negative electrode contains at least each active material and a composite compound. The composite compound preferably has crystallinity, for example, molecular crystals.
[0016] In a secondary battery, the composite compound preferably functions as a binder and exhibits high ionic conductivity.
[0017] In a secondary battery, it is preferable that the composite compound functions as a solid electrolyte in addition to a binder. When the composite compound functions as a solid electrolyte, the secondary battery does not need to have a separator. It is preferable that the composite compound is arranged so that each active material does not come into contact with the organic electrolyte (a liquid one is called an electrolyte solution). For example, it is preferable that the composite compound is arranged so as to cover a portion of each active material.
[0018] A specific embodiment of the present invention is a secondary battery having a positive electrode and a negative electrode, in which one or both of the positive electrode and the negative electrode have an active material and a composite compound having a crystalline structure, and the composite compound functions as a binder.
[0019] Another embodiment of the present invention is a secondary battery having a positive electrode, a negative electrode, and an electrolyte, in which one or both of the positive electrode and the negative electrode have an active material and a composite compound having a crystalline structure, the composite compound functions as a binder, and the composite compound has a region located between the active material and the electrolyte.
[0020] Another embodiment of the present invention is a secondary battery having a positive electrode and a negative electrode, in which one or both of the positive electrode and the negative electrode have an active material and a composite compound having a crystalline structure, and the composite compound functions as a binder and an electrolyte.
[0021] Another embodiment of the present invention is a secondary battery including a positive electrode and a negative electrode, in which one or both of the positive electrode and the negative electrode includes an active material, a composite compound having a crystalline structure, and a first binder, and the composite compound functions as a second binder and an electrolyte.
[0022] Another aspect of the present invention is a secondary battery having a positive electrode and a negative electrode, wherein one or both of the positive electrode and the negative electrode has an active material and a composite compound having a crystalline structure, the composite compound functions as a binder, and the composite compound has succinonitrile, lithium ions, and bis(fluorosulfonyl)imide ions.
[0023] Another embodiment of the present invention is a secondary battery having a positive electrode and a negative electrode, in which one or both of the positive electrode and the negative electrode have an active material and a composite compound having a crystalline structure, the composite compound functions as a binder, and the composite compound has glutaronitrile, lithium ions, and bis(fluorosulfonyl)imide ions.
[0024] Another embodiment of the present invention is a secondary battery having a positive electrode and a negative electrode, in which one or both of the positive electrode and the negative electrode have an active material and a composite compound having a crystalline structure, the composite compound functions as a binder, and the composite compound has adiponitrile, lithium ions, and bis(fluorosulfonyl)imide ions.
[0025] Another embodiment of the present invention is a secondary battery having a positive electrode, a negative electrode, and an electrolyte, in which one or both of the positive electrode and the negative electrode have an active material and a composite compound having a crystalline structure, the composite compound functions as a binder, and the composite compound has a region located between the active material and the electrolyte, and the composite compound has succinonitrile, lithium ions, and bis(fluorosulfonyl)imide.
[0026] Another embodiment of the present invention is a secondary battery having a positive electrode, a negative electrode, and an electrolyte, in which one or both of the positive electrode and the negative electrode have an active material and a composite compound having a crystalline structure, the composite compound functions as a binder, and the composite compound has a region located between the active material and the electrolyte, and the composite compound has glutaronitrile, lithium ions, and bis(fluorosulfonyl)imide.
[0027] Another aspect of the present invention is a secondary battery having a positive electrode, a negative electrode, and an electrolyte, in which one or both of the positive electrode and the negative electrode have an active material and a composite compound having a crystalline structure, the composite compound functions as a binder, and the composite compound has a region located between the active material and the electrolyte, and the composite compound has adiponitrile, lithium ions, and bis(fluorosulfonyl)imide ions.
[0028] Another aspect of the present invention is a secondary battery having a positive electrode and a negative electrode, wherein one or both of the positive electrode and the negative electrode has an active material and a composite compound having a crystalline structure, the composite compound functions as a binder and an electrolyte, and the composite compound has succinonitrile, lithium ions, and bis(fluorosulfonyl)imide ions.
[0029] Another embodiment of the present invention is a secondary battery having a positive electrode and a negative electrode, in which one or both of the positive electrode and the negative electrode have an active material and a composite compound having a crystalline structure, the composite compound functions as a binder and an electrolyte, and the composite compound has glutaronitrile, lithium ions, and bis(fluorosulfonyl)imide ions.
[0030] Another embodiment of the present invention is a secondary battery having a positive electrode and a negative electrode, in which one or both of the positive electrode and the negative electrode have an active material and a composite compound having a crystalline structure, the composite compound functions as a binder and an electrolyte, and the composite compound has adiponitrile, lithium ions, and bis(fluorosulfonyl)imide.
[0031] In one embodiment of the present invention, the active material of the positive electrode preferably includes a composite oxide containing magnesium and cobalt, with cobalt present inside and in a surface layer portion of the active material and magnesium present at least in the surface layer portion.
[0032] In one embodiment of the present invention, the active material of the positive electrode preferably has a surface roughness of at least less than 3 nm when surface roughness information is quantified in a cross section observed with a scanning transmission electron microscope (STEM).
[0033] In one embodiment of the present invention, it is preferable to have a separator between the positive electrode and the negative electrode.
[0034] In one embodiment of the present invention, the active material of the positive electrode preferably has a layered rock salt type crystal structure.
[0035] In one embodiment of the present invention, the active material of the negative electrode preferably contains silicon or carbon.
[0036] In one embodiment of the present invention, it is preferable that either or both of the positive electrode and the negative electrode contain a conductive material.
[0037] In one embodiment of the present invention, the conductive material contained in the positive electrode preferably includes carbon black, graphene, or carbon nanotubes.
[0038] In one embodiment of the present invention, the conductive material contained in the negative electrode preferably includes carbon black, graphene, or carbon nanotubes.
[0039] Another embodiment of the present invention is a power storage system including the above secondary battery and a protection circuit.
[0040] Another aspect of the present invention is a vehicle equipped with the above secondary battery.
[0041] One aspect of the present invention is a method for producing a positive electrode, the method including a first step and a second step, in which the first step comprises heating a composite compound having a crystalline structure and a positive electrode active material while mixing them to produce a positive electrode slurry, and the second step comprises applying the positive electrode slurry to a current collector, the heating being performed at a temperature equal to or higher than the melting point of the composite compound having a crystalline structure.
[0042] Another aspect of the present invention is a method for producing a positive electrode, the method including a first step and a second step, in which the first step comprises heating a first compound, a second compound, and a positive electrode active material while mixing them to produce a positive electrode slurry, and the second step comprises applying the positive electrode slurry to a current collector, the heating in the first step being performed at a temperature equal to or higher than the melting points of the first compound and the second compound.
[0043] Another embodiment of the present invention is a method for manufacturing a positive electrode, the method including first to third steps, in which the first step includes heating a first compound and a second compound while mixing them to form a composite compound having a crystalline structure, the second step includes heating a positive electrode active material and the composite compound while mixing them to form a positive electrode slurry, and the third step includes applying the positive electrode slurry to a current collector, wherein the heating in the first step is performed at a temperature equal to or higher than a melting point of the composite compound.
[0044] In one embodiment of the present invention, the first compound preferably comprises succinonitrile, glutaronitrile, or adiponitrile, and the second compound preferably comprises lithium bis(fluorosulfonyl)imide.
[0045] Another aspect of the present invention is a method for manufacturing a positive electrode, the method including first to fifth steps, in which the first step includes mixing a first binder mixture with a conductive material to prepare a first mixture, the second step includes mixing the first mixture with a positive electrode active material to prepare a second mixture, the third step includes mixing the second mixture with the second binder mixture and a dispersion medium to prepare a third mixture, the fourth step includes applying the third mixture to a current collector and drying the dispersion medium to prepare a coated electrode, and the fifth step includes injecting, while heating, a composite compound having a crystalline structure into voids in the coated electrode.
[0046] In one embodiment of the present invention, the composite compound having a crystalline structure is preferably obtained by heating succinonitrile, glutaronitrile, or adiponitrile and lithium bis(fluorosulfonyl)imide while mixing them.
[0047] According to one embodiment of the present invention, a highly reliable or safe secondary battery and a manufacturing method thereof can be provided. Alternatively, a secondary battery with excellent charge-discharge cycle characteristics and a manufacturing method thereof can be provided. Alternatively, a secondary battery with large discharge capacity and a manufacturing method thereof can be provided.
[0048] In order to realize the above secondary battery, one embodiment of the present invention can provide a positive electrode or a negative electrode that is stable in a high potential state and / or a high temperature state, and a manufacturing method thereof.
[0049] To realize the above-described positive electrode or negative electrode, it is possible to provide a positive electrode active material or negative electrode active material whose crystalline structure is not easily destroyed even after repeated charge and discharge, and a method for manufacturing the same. Alternatively, it is possible to provide a positive electrode active material or negative electrode active material with excellent charge and discharge cycle characteristics, and a method for manufacturing the same. Alternatively, it is possible to provide a positive electrode active material or negative electrode active material with a large discharge capacity, and a method for manufacturing the same.
[0050] Note that the description of these effects does not preclude the existence of other effects. Note that one embodiment of the present invention does not necessarily have all of these effects. Note that effects other than these will become apparent from the description in the specification, drawings, claims, etc., and it is possible to extract other effects from the description in the specification, drawings, claims, etc.
[0051] FIGS. 1A to 1C4 are diagrams illustrating a secondary battery of one embodiment of the present invention. FIGS. 2A and 2B are diagrams illustrating a secondary battery of one embodiment of the present invention. FIGS. 3A and 3B are diagrams illustrating an example of a method for manufacturing a positive electrode used in a lithium-ion secondary battery of one embodiment of the present invention. FIGS. 4A and 4B are diagrams illustrating an example of a method for manufacturing a positive electrode used in a lithium-ion secondary battery of one embodiment of the present invention. FIGS. 5A and 5B are diagrams illustrating an example of a method for manufacturing a lithium-ion secondary battery of one embodiment of the present invention. FIGS. 6A to 6C are diagrams illustrating an example of a method for manufacturing a cathode active material composite of one embodiment of the present invention. FIGS. 7A and 7B are models calculated by density functional theory for a cathode active material composite of one embodiment of the present invention. FIGS. 8A to 8C are graphs of calculation results by density functional theory for a cathode active material composite of one embodiment of the present invention. FIGS. 9A to 9C are diagrams illustrating a method for manufacturing a cathode active material of one embodiment of the present invention. FIG. 10 is a diagram illustrating a method for manufacturing a cathode active material of one embodiment of the present invention. FIGS. 11A to 11C are diagrams illustrating a method for manufacturing a cathode active material of one embodiment of the present invention. FIG. 12A is a front view of a cathode active material of one embodiment of the present invention, and FIG. 12B is a cross-sectional view of the cathode active material of one embodiment of the present invention. FIG. 13 is a diagram illustrating a crystal structure of a cathode active material of one embodiment of the present invention. FIG. 14 is an XRD pattern calculated from the crystal structure. FIG. 15 is a diagram illustrating the crystal structure of a conventional cathode active material. FIG. 16 is an XRD pattern calculated from the crystal structure. FIGS. 17A to 17C are lattice constants calculated from the XRD patterns. FIGS. 18A to 18C are lattice constants calculated from the XRD patterns. FIG. 19 is a graph showing charge curves of secondary batteries using a cathode active material of one embodiment of the present invention and a comparative cathode active material. FIGS. 20A and 20B are dQ / dV curves of half cells of one embodiment of the present invention, and FIG. 20C is a dQ / dV curve of a comparative half cell. Fig. 21 is a cross-sectional schematic diagram of the positive electrode active material, and Fig. 22A and Fig. 22B are SEM images of the positive electrode.FIG. 23A is a front view of the positive electrode active material based on FIB (Focused Ion Beam) processing and SEM observation, FIG. 23B is an enlarged view of a portion thereof, FIG. 23C is a cross-sectional view thereof, FIG. 23D is a rotated side view of the positive electrode active material of FIG. 23A, FIG. 23E is an enlarged view of a portion thereof, and FIG. 23F is a cross-sectional view thereof. FIGS. 24A to 24C are SEM images of the positive electrode. FIGS. 25A to 25C are SEM images of the positive electrode. FIGS. 26A and 26B are STEM images of the positive electrode. FIGS. 27A to 27C are EDX analysis results of the positive electrode. FIGS. 28A and 28B are cross-sectional TEM images of the positive electrode active material layer. FIGS. 29A to 29C are microelectron diffraction patterns of the positive electrode active material layer. FIGS. 30A to 30C are diagrams showing examples of crystal structures. FIG. 31A is an STEM photograph of the particles after pressing, and FIGS. 31B and 31C are cross-sectional schematic views. FIG. 32A is an exploded perspective view of a coin-type secondary battery, FIG. 32B is a perspective view of the coin-type secondary battery, and FIG. 32C is a cross-sectional perspective view thereof. FIG. 33A shows an example of a cylindrical secondary battery. FIG. 33B shows an example of a cylindrical secondary battery. FIG. 33C shows an example of multiple cylindrical secondary batteries. FIG. 33D shows an example of an energy storage system having multiple cylindrical secondary batteries. FIGS. 34A and 34B are diagrams illustrating an example of a secondary battery, and FIG. 34C is a diagram illustrating the internal state of the secondary battery. FIGS. 35A to 35C are diagrams illustrating an example of a secondary battery. FIGS. 36A and 36B are diagrams illustrating the external appearance of a secondary battery. FIGS. 37A to 37C are diagrams illustrating a method for fabricating a secondary battery. FIGS. 38A to 38C are diagrams illustrating an example of the configuration of a battery pack. FIGS. 39A and 39B are diagrams illustrating an example of a secondary battery. 40A to 40C are diagrams illustrating an example of a secondary battery. FIGS. 41A and 41B are diagrams illustrating an example of a secondary battery. FIG. 42A is a perspective view of a battery pack illustrating one embodiment of the present invention, FIG. 42B is a block diagram of the battery pack, and FIG. 42C is a block diagram of a vehicle having a motor. FIGS. 43A to 43D are diagrams illustrating an example of a transportation vehicle. FIGS. 44A and 44B are diagrams illustrating a power storage device of one embodiment of the present invention. FIG. 45A is a diagram illustrating an electric bicycle, FIG. 45B is a diagram illustrating a secondary battery for the electric bicycle, and FIG. 45C is a diagram illustrating an electric motorcycle.46A to 46D are diagrams illustrating an example of an electronic device. FIG. 47A shows an example of a wearable device, FIG. 47B shows a perspective view of a wristwatch-type device, and FIG. 47C is a diagram illustrating a side view of the wristwatch-type device. FIG. 47D is a diagram illustrating an example of a wireless earphone. FIG. 48A to FIG. 48C are diagrams illustrating the structural formula of a compound and the magnitude of the charge of each nitrogen atom. FIG. 49A to FIG. 49C are diagrams illustrating an example of a stable structure of a complex compound. FIG. 50A is a diagram illustrating a method for preparing a complex compound, FIG. 50B is a photograph of the prepared complex compound, and FIG. 50C is a diagram illustrating the analysis results. FIG. 51A is a diagram illustrating a method for preparing a complex compound, FIG. 51B is a photograph of the prepared complex compound, and FIG. 51C is a diagram illustrating the analysis results.
[0052] Hereinafter, embodiments of the present invention will be described in detail with reference to the drawings. However, the present invention is not limited to the following description, and it will be readily understood by those skilled in the art that various modifications can be made to the embodiments and details. Furthermore, the present invention should not be interpreted as being limited to the description of the embodiments shown below.
[0053] In this specification and the like, a secondary battery has, for example, a positive electrode and a negative electrode. The positive electrode has a positive electrode active material. The positive electrode active material is, for example, a substance that undergoes a reaction that contributes to charge / discharge capacity. Note that the positive electrode active material may partially contain a substance that does not contribute to charge / discharge capacity.
[0054] In this specification etc., the positive electrode active material may be expressed as a positive electrode material, a positive electrode material for secondary batteries, a composite oxide, or the like. Also in this specification etc., the positive electrode active material preferably has a compound corresponding to the composite oxide. Also in this specification etc., the positive electrode active material preferably has a composition corresponding to the composite oxide. Also in this specification etc., the positive electrode active material preferably has a composite corresponding to the composite oxide.
[0055] In this specification and the like, the term "particles" is not limited to referring only to spherical particles (having a circular cross-sectional shape), but also includes particles having a cross-sectional shape such as an ellipse, rectangle, trapezoid, square with rounded corners, or asymmetric shape, and further, individual particles may have an irregular shape.
[0056] In this specification and the like, particle size can be measured by, for example, laser diffraction particle size distribution measurement, and can be compared using the D50 value. Here, D50 is the particle size when the cumulative amount in the cumulative particle amount curve of the particle size distribution measurement result accounts for 50%, i.e., the median. Measurement of particle size is not limited to laser diffraction particle size distribution measurement, and when the particle size is below the lower measurement limit of laser diffraction particle size distribution measurement, the major axis of the particle cross section may be measured by analysis such as SEM (Scanning Electron Microscope) or TEM (Transmission Electron Microscope).
[0057] In this specification and elsewhere, Miller indices are used to represent crystal planes and directions. Individual planes representing crystal planes are represented in parentheses. In crystallography, crystal planes, directions, and space groups are represented by placing a superscript bar above the numbers, but in this specification and elsewhere, due to limitations on application notation, numbers may be represented by placing a - (minus sign) before them instead of placing a bar above them.
[0058] In this specification, the layered rock-salt type crystal structure of a composite oxide containing lithium and a transition metal has a rock-salt type ion arrangement in which cations and anions are arranged alternately. In the layered rock-salt type crystal structure, the transition metal and lithium are regularly arranged to form a two-dimensional plane, allowing two-dimensional diffusion of lithium. Note that the layered rock-salt type crystal structure may have defects such as cation or anion deficiencies. Furthermore, the layered rock-salt type crystal structure may have a structure in which the rock-salt type crystal lattice is distorted.
[0059] In this specification, the rock salt type crystal structure refers to a structure in which cations and anions are arranged alternately. Note that the crystal structure may have defects such as missing cations or anions.
[0060] In this specification, the theoretical capacity of a positive electrode active material refers to the amount of electricity when all of the intercalable and deintercalable lithium contained in the positive electrode active material is deintercalated. 4 The theoretical capacity of LiCoO is 170 mAh / g. 2 The theoretical capacity of LiNiO is 274 mAh / g. 2 The theoretical capacity of LiMn is 274mAh / g.2 O 4 The theoretical capacity of the battery is 148 mAh / g.
[0061] In this specification and the like, the amount of lithium remaining in the positive electrode active material that can be inserted and removed is determined by x in the composition formula, for example, Li x CoO 2 x in, or Li x MO 2 In this specification, Li x CoO 2 Li as appropriate x MO 2 In the case of a positive electrode active material in a secondary battery, x can be expressed as x = (theoretical capacity - charging capacity) / theoretical capacity. For example, LiCoO 2 When a secondary battery using as a positive electrode active material is charged at 219.2 mAh / g, Li 0.2 CoO 2 Or we can say x = 0.2. x CoO 2 The small value of x in the formula means, for example, 0.1<x≦0.24.
[0062] When properly synthesized lithium cobalt oxide is used in the positive electrode, the stoichiometric ratio is approximately satisfied. 2 and the occupancy rate of Li on the lithium site is x = 1. In addition, the secondary battery after discharge is also LiCoO 2 It can be said that x = 1. The completion of discharge here refers to a state in which the voltage becomes 2.5 V (lithium counter electrode) or less at a current of, for example, 100 mA / g.
[0063] In this specification and the like, when evaluating a positive electrode and a positive electrode active material, cycle test examples using lithium metal as the counter electrode are sometimes shown, but one embodiment of the present invention is not limited to this. Instead of lithium metal, graphite, lithium titanate, or the like may be used. That is, the properties of the positive electrode and the positive electrode active material, such as the ability to maintain their crystalline structure even after repeated charge and discharge and to obtain good cycle characteristics, are not affected by the material of the negative electrode.
[0064] In this specification, a cycle test is a test in which charging and discharging are repeated. The cycle test can observe the degree of deterioration of a secondary battery and can evaluate the positive electrode and the positive electrode active material.
[0065] In this specification and the like, examples of secondary batteries in which the secondary battery is charged and discharged at a relatively high voltage of 4.6 V using a lithium counter electrode are sometimes shown, but the secondary battery may be charged and discharged at a voltage lower than the charging voltage of 4.6 V. When the secondary battery is charged and discharged at a lower voltage, it is expected that the cycle characteristics will be even better than those shown in this specification and the like.
[0066] In this specification, the term "kiln" refers to a device for heating an object to be treated. For example, the term "kiln" may be replaced with a furnace, a kiln, a heating device, or the like.
[0067] In this embodiment, a secondary battery according to one embodiment of the present invention will be described. The secondary battery includes a positive electrode and a negative electrode according to one embodiment of the present invention. Note that a secondary battery using lithium ions as carrier ions is called a lithium-ion secondary battery.
[0068] 1A shows a cross-sectional view of a secondary battery 100. The secondary battery 100 has a positive electrode 101 and a negative electrode 102. A separator 110 is located between the positive electrode 101 and the negative electrode 102. In other words, the positive electrode 101 and the negative electrode 102 are separated by the separator 110. Note that the separator 110 may not be provided as long as the positive electrode 101 and the negative electrode 102 can be maintained separated.
[0069] The positive electrode 101 includes a positive electrode current collector 104 and a positive electrode active material layer 105. The positive electrode active material layer 105 includes a positive electrode active material. The positive electrode active material includes an active material capable of absorbing and releasing carrier ions. For example, the active material may be LiMO. 2 (M1 is one or more selected from Fe, Ni, Co, Mn, and Al) can be used. The composite oxide is, for example, one that uses a first oxide and a second oxide as starting materials, and the term "composite" may mean that two or more oxides are used as starting materials. Specific composite oxides will be described later in this embodiment.
[0070] The positive electrode active material is disposed in a state capable of donating and receiving electrons to and from the positive electrode current collector 104. That is, the positive electrode active material is configured to be in electrical contact with the positive electrode current collector 104. An undercoat layer may be provided on the positive electrode current collector 104. In this case, the positive electrode active material is configured to be in electrical contact with the positive electrode current collector 104 via the undercoat layer. The positive electrode active material may also be configured to be in electrical contact with the positive electrode current collector 104 via a conductive material. The conductive material is also called a conductive additive, and is a material having a lower resistivity than the positive electrode active material. The conductive material can form an efficient current path between the positive electrode active material and the positive electrode current collector, or between the positive electrode active materials themselves. For this reason, it is preferable that the conductive material be present in a moderately dispersed state in the positive electrode active material layer 105.
[0071] The negative electrode 102 includes a negative electrode current collector 106 and a negative electrode active material layer 107. The negative electrode active material layer 107 includes a negative electrode active material. The negative electrode active material includes an active material capable of absorbing and releasing carrier ions. Specific examples of the negative electrode active material will be described in the following embodiments.
[0072] The negative electrode active material is disposed in a state capable of donating and receiving electrons to and from the negative electrode current collector 106. That is, the negative electrode active material is in electrical contact with the negative electrode current collector 106. An undercoat layer may be provided on the negative electrode current collector 106. In this case, the negative electrode active material is in electrical contact with the negative electrode current collector 106 via the undercoat layer. The negative electrode active material may also be in electrical contact with the negative electrode current collector 106 via a conductive material. The conductive material is also called a conductive additive, and is a material having a lower resistivity than the negative electrode active material. The conductive material can form an efficient current path between the negative electrode active material and the negative electrode current collector, or between the negative electrode active materials themselves. Therefore, it is preferable that the conductive material be present in a moderately dispersed state in the negative electrode active material layer 107.
[0073] The structure of the positive electrode active material and its vicinity will be described. Fig. 1B1 corresponds to an enlarged view of region 112 in Fig. 1A, and shows at least an electrolyte (a liquid electrolyte is called an electrolyte solution) 114 and a positive electrode active material 115. The positive electrode active material 115 is preferably covered with a composite compound 117.
[0074] The composite compound 117 is made from, for example, a first compound and a second compound as starting materials, and the term "composite" may mean that two or more compounds are used as starting materials. The composite compound preferably has a crystalline structure.
[0075] The composite compound having a crystalline structure may be, for example, a molecular crystal. Molecular crystal is a general term for a crystal of a molecular composite compound formed by bonding Compound A and Compound B through physical intermolecular forces, such as coordinate bonds. The molecular crystal is formed by mixing a first compound and a second compound, and may have a structure in which parts of the compounds are bonded together through coordinate bonds.
[0076] The composite compound 117 can function as a binder for the positive electrode active material 115. The composite compound 117 may function as a binder for the positive electrode active material 115 in addition to the binder contained in the positive electrode active material layer.
[0077] The composite compound 117 may preferably contain a material with high ionic conductivity, so that carrier ions can be transferred between the positive electrode active material 115 and the electrolyte 114 via the composite compound 117. In other words, the composite compound 117 can function as an electrolyte.
[0078] Furthermore, the composite compound 117 can function as both a binder and an electrolyte.
[0079] The composite compound 117 having a crystalline structure is in a solid state. When the composite compound 117 having a crystalline structure is used as an electrolyte, a separator can be eliminated. In other words, a secondary battery using the composite compound 117 having a crystalline structure as an electrolyte can have the same configuration as an all-solid-state secondary battery.
[0080] Furthermore, by being covered with the composite compound 117, the positive electrode active material 115 can have a region that is not in contact with the electrolyte 114. In this case, the composite compound 117 is arranged so as to have a region that is located between the positive electrode active material 115 and the electrolyte 114. It is believed that such composite compound 117 suppresses deterioration of the positive electrode active material 115 caused by the electrolyte 114.
[0081] The above-mentioned deterioration will now be explained. It is believed that the deterioration occurs due to defects in the positive electrode active material 115. These defects include those called cracks or pits. During charging and discharging of a secondary battery, the positive electrode active material 115 repeatedly expands and contracts. The volume change associated with this expansion and contraction is believed to exert physical pressure on the positive electrode active material 115. This pressure is believed to result in defects, such as cracks. A crack refers to a break caused by the application of physical pressure. A pit refers to a hole formed by the loss of several layers of a main component, such as cobalt or oxygen, and includes holes caused by pitting corrosion. For example, cobalt is believed to dissolve into the electrolyte 114, and the dissolution of one layer of cobalt can result in a hole. This is called a pit. Pits can progress during charging and discharging of a secondary battery, eventually becoming deeper. In other words, pits can be considered progressive defects.
[0082] The composite compound 117 provides a configuration in which the electrolyte 114 and the positive electrode active material 115 are not in contact with each other, thereby suppressing the occurrence and progression of the defects that can cause deterioration, such as pits. To achieve the effect of suppressing deterioration, the composite compound 117 only needs to cover a portion of the positive electrode active material 115. With this configuration, deterioration of the secondary battery can be suppressed.
[0083] Another positive electrode active material and its surrounding structure will now be described. FIG. 1B2 corresponds to an enlarged view of region 112 in FIG. 1A, and shows at least a positive electrode active material 115 covered with a conductive material 118 and a barrier layer 116. A positive electrode active material covered with a barrier layer may be referred to as a positive electrode active material composite, and the positive electrode active material composite will be described in embodiment 3 and the like. The other structure of FIG. 1B2 is the same as that of FIG. 1B1. The barrier layer 116 exists as a region containing a material different from the main active material material of the positive electrode active material 115. The barrier layer 116 also exists as a region containing an additive element contained in the positive electrode active material 115. Specific materials used for the additive element will be described in the following embodiments.
[0084] The barrier layer 116 is preferably located in the surface layer portion of the positive electrode active material 115. The surface layer portion refers to, for example, a region within 50 nm from the surface of the positive electrode active material toward the inside, more preferably within 35 nm from the surface toward the inside, even more preferably within 20 nm from the surface toward the inside, and most preferably within 10 nm from the surface toward the inside. Surfaces caused by cracks and / or fissures may also be considered to be the surface.
[0085] The presence of the barrier layer 116 in the surface layer portion can suppress deterioration over time of the positive electrode active material 115. To suppress deterioration over time, it is preferable that the barrier layer 116 covers the entire surface of the positive electrode active material 115, but it goes without saying that the deterioration suppression effect can also be achieved by the barrier layer 116 covering only a part of the positive electrode active material 115.
[0086] After forming the positive electrode active material 115 having the barrier layer 116 on its surface, the composite compound 117 may be provided on the positive electrode active material 115. That is, the composite compound 117 may be located outside the barrier layer 116. This is to prevent the positive electrode active material 115 from contacting the electrolyte 114 by the composite compound 117. Furthermore, the composite compound 117 may have a region that is thicker than the barrier layer 116.
[0087] The conductive material 118 is disposed to enhance the conductivity of the positive electrode active material 115. Therefore, the conductive material 118 includes a material having a higher conductivity than the positive electrode active material 115. Specific materials used for the conductive material will be described later in this embodiment.
[0088] The conductive material 118 can serve as a current path between the positive electrode active material 115 and the positive electrode current collector 104. The conductive material 118 may be mixed into the composite compound 117. In the mixed region, the composite compound 117 may be torn, and the positive electrode active material 115 may be exposed from the composite compound 117. The conductive material 118 may be applied to the configuration shown in FIG. 1B1 above.
[0089] Another configuration of the positive electrode active material and its vicinity will be described. FIG. 1B3 corresponds to an enlarged view of region 112 in FIG. 1A, and shows a state in which at least a first positive electrode active material 115a and a second positive electrode active material 115b are bonded. The other configurations of FIG. 1B3 are the same as those of FIG. 1B2. As another configuration of FIG. 1B3, a barrier layer may be provided on the surface layer portions of the first positive electrode active material 115a and the second positive electrode active material 115b, as shown in FIG. 1B2.
[0090] Because the first positive electrode active material 115a and the second positive electrode active material 115b are bonded together, the composite compound 117 covers both the first positive electrode active material 115a and the second positive electrode active material 115b. If a barrier layer is provided, the composite compound 117 is preferably located outside the barrier layer. It can be considered that the composite compound 117 prevents the first positive electrode active material 115a and the second positive electrode active material 115b from contacting the electrolyte 114, and deterioration of the first positive electrode active material 115a and the second positive electrode active material 115b due to the electrolyte 114 is suppressed.
[0091] Next, the structure of the negative electrode active material and its vicinity will be described. FIG. 1C1 corresponds to an enlarged view of region 113 in FIG. 1A and shows at least the electrolyte 114 and the first negative electrode active material 125. The electrolyte 114 is also included in the positive electrode 101. The first negative electrode active material 125 is preferably covered with a composite compound 127. The composite compound 127 can function as a binder for the first negative electrode active material 125. The composite compound 127 preferably contains a material with high ionic conductivity, and the first negative electrode active material 125 covered with the composite compound 127 can exchange carrier ions with the electrolyte 114 via the composite compound 127. In other words, the composite compound 127 can function as an electrolyte.
[0092] The composite compound 127 may contain the same material as the composite compound 117 contained in the positive electrode, or may contain a material different from that of the composite compound 117 contained in the positive electrode.
[0093] The composite compound 127 is a composite compound made from a first compound and a second compound as starting materials, and the term "composite" may refer to the use of two or more compounds as starting materials. The composite compound preferably has a crystalline structure. A composite compound having a crystalline structure has a high function of retaining the first negative electrode active material 125 and is suitable for use as a binder. A composite compound having a crystalline structure is also suitable as an electrolyte, and functions as a so-called solid electrolyte, making a separator unnecessary.
[0094] The complex compound having a crystalline structure may be, for example, a molecular crystal.
[0095] Furthermore, the first negative electrode active material 125 covered with the complex compound 127 can be disposed so as not to come into contact with the electrolyte 114. Therefore, deterioration of the first negative electrode active material 125 due to the electrolyte is suppressed.
[0096] To suppress the deterioration, the complex compound 127 only needs to cover a part of the first negative electrode active material 125. With such a structure, deterioration of the secondary battery can be suppressed.
[0097] Another negative electrode active material and its surrounding structure will now be described. Fig. 1C2 corresponds to an enlarged view of region 113 in Fig. 1A, and shows at least first negative electrode active material 125a and second negative electrode active material 125b bonded together. The other structure in Fig. 1C2 is similar to that in Fig. 1C1.
[0098] Because the first negative electrode active material 125 a and the second negative electrode active material 125 b are bonded together, the composite compound 127 has a structure in which both the first negative electrode active material 125 a and the second negative electrode active material 125 b are covered. It can be considered that the composite compound 127 prevents the first negative electrode active material 125 a and the second negative electrode active material 125 b from contacting the electrolyte 114, and deterioration of the first negative electrode active material 125 a and the second negative electrode active material 125 b due to the electrolyte is suppressed.
[0099] Another configuration of the negative electrode active material and its vicinity will now be described. Fig. 1C3 corresponds to an enlarged view of region 113 in Fig. 1A, and shows at least first negative electrode active material 125a and second negative electrode active material 125b bonded together, and further shows conductive material 128. The other configurations in Fig. 1C3 are similar to those in Fig. 1C2.
[0100] The conductive material 128 is disposed to enhance the conductivity of the first negative electrode active material 125. Therefore, the conductive material 128 includes a material having higher conductivity than the first negative electrode active material 125. Specific materials used for the conductive material will be described later in this embodiment.
[0101] The conductive material 128 can serve as a current path between the first negative electrode active material 125 and the negative electrode current collector 106. In FIG. 1C3 , it is considered that the conductive material 128 also serves as a current path between the first negative electrode active material 125 a and the second negative electrode active material 125 b. The conductive material 128 may be mixed into the composite compound 127. In the mixed region, the composite compound 127 may be torn, and parts of the first negative electrode active material 125 a and the second negative electrode active material 125 b may be exposed from the composite compound 127.
[0102] Another configuration of the negative electrode active material and its vicinity will now be described. FIG. 1C4 corresponds to an enlarged view of region 113 in FIG. 1A, and shows at least a first negative electrode active material 125 and a second negative electrode active material 129. A plurality of first negative electrode active materials 125 and a plurality of second negative electrode active materials 129 are shown. The first negative electrode active material 125 preferably has a different material or particle size from the second negative electrode active material 129. For example, the first negative electrode active material 125 may be nanoparticles containing silicon and having a small particle size, while the second negative electrode active material 129 may contain graphite, and the particle size of the second negative electrode active material 129 may be larger than that of the first negative electrode active material 125. The other configurations in FIG. 1C4 are similar to those in FIG. 1C3.
[0103] Next, an example of the configuration of a secondary battery that combines any one of the above-described positive electrode active materials with any one of the above-described negative electrode active materials will be described. FIG. 2A shows a cross-sectional view of a secondary battery 100. The secondary battery 100 is an example that uses the positive electrode active material described in FIG. 1B2 and the negative electrode active material described in FIG. 1C4. In this way, any one of the above-described positive electrode active materials and any one of the above-described negative electrode active materials can be combined and used in a secondary battery.
[0104] The separator 110 is permeated with an electrolyte 114. The permeated state is sometimes referred to as impregnation.
[0105] Furthermore, the positive electrode active material 115 covered with the composite compound 117, and the first negative electrode active material 125 and second negative electrode active material 129 covered with the composite compound 127 have regions that do not come into contact with the electrolyte 114, thereby suppressing electrolyte-induced deterioration of the positive electrode active material 115, the first negative electrode active material 125, and the second negative electrode active material 129. This deterioration is thought to be caused by defects that occur in the positive electrode active material 115, the first negative electrode active material 125, and the second negative electrode active material 129. These defects include cracks and pits. The configuration in which the electrolyte 114 does not come into contact with the positive electrode active material 115, the first negative electrode active material 125, and the second negative electrode active material 129 can suppress the occurrence and progression of the defects, particularly pits.
[0106] In order to suppress the deterioration, it is sufficient that the positive electrode active material 115, the first negative electrode active material 125, and the second negative electrode active material 129 have regions that are not in contact with the electrolyte 114, and therefore the composite compound 117 does not need to cover all of the positive electrode active material 115, the first negative electrode active material 125, and the second negative electrode active material 129 as long as it covers only a part of them. With such a configuration, it is possible to suppress the occurrence and progression of the defects, particularly pits, and to suppress deterioration of the secondary battery.
[0107] The composite compound 117 functions to bind multiple positive electrode active materials 115 together and thus functions as a binder. The composite compound 117 functions to bind the positive electrode current collector 104 and the positive electrode active materials 115 together and thus functions as a binder. The composite compound 117 may have a region mixed with a conductive material 118. When the conductivity of the composite compound 117 is low, the conductive material 118 can ensure a current path. On the surface of the positive electrode current collector 104, the positive electrode active materials 115 or the composite compound 117 may be pressed into a state. That is, the surface of the positive electrode current collector 104 may have unevenness in a cross-sectional view of the secondary battery. Furthermore, on the surface of the positive electrode current collector 104, the composite compound 117 may break, and the positive electrode active material 115 may be exposed from the composite compound 117. The exposed region is in contact with the positive electrode current collector 104 and is therefore considered not to come into contact with the electrolyte 114.
[0108] The composite compound 127 functions as a binder, binding the first anode active materials 125 together, the second anode active materials 129 together, or the first anode active material 125 and the second anode active material 129 together. The composite compound 127 functions as a binder, binding the anode current collector 106 to the first anode active material 125 or the second anode active material 129. The composite compound 127 may have a region where a conductive material 128 is mixed. When the conductivity of the composite compound 127 is low, a current path can be secured by the conductive material 128. On the surface of the anode current collector 106, the first anode active material 125, the second anode active material 129, or the composite compound 127 may be pressed into the surface. That is, the surface of the anode current collector 106 may have unevenness in a cross-sectional view of the secondary battery. Furthermore, on the surface of the negative electrode current collector 106, the composite compound 127 may be broken, and the first negative electrode active material 125 or the second negative electrode active material 129 may be exposed from the composite compound 127. The exposed region is in contact with the negative electrode current collector 106 and is therefore not considered to be in contact with the electrolyte 114.
[0109] The composite compound 127 may have the same material as the composite compound 117 or a different material. The composite compound 117 and the composite compound 127 may have any material as long as they have a crystalline structure, and it is more preferable that they have high ionic conductivity. When the ionic conductivity is high, the composite compound 117 and the composite compound 127 can function as an electrolyte.
[0110] The composite compound 117 or the composite compound 127 can be obtained using a first compound and a second compound as starting materials.
[0111] The first compound has a compound represented by the following general formula (G1): The following general formula (G1) is a compound having a cyano group.
[0112]
[0113] In the general formula (G1), R represents a hydrocarbon having 1 to 5 carbon atoms. Preferably, in the general formula (G1), R represents a hydrocarbon having 2 to 4 carbon atoms.
[0114] Specific examples of the compound represented by the general formula (G1) include succinonitrile, glutaronitrile, and adiponitrile, and a specific example of the compound having a cyano group includes acetonitrile. One or more compounds selected from these can be used as the first compound.
[0115] The second compound is lithium bis(fluorosulfonyl)imide (Li(FSO 2 ) 2 N, abbreviated as LiFSI), lithium bis(trifluoromethanesulfonyl)imide (Li(CF 3 SO 2 ) 2 N, abbreviated as LiTFSI), and lithium bis(pentafluoroethanesulfonyl)imide (Li(C 2 F 5 SO 2 ) 2 N, abbreviated as LiBETI), one or more selected from the group consisting of:
[0116] Preferred examples of combinations of the first compound and the second compound are shown in the following (H1) to (H3).
[0117]
[0118]
[0119]
[0120] Whether the composite compound obtained by combining the compounds shown in (H1) to (H3) above forms a molecular crystal can be confirmed by XRD measurement, etc. In the results of the XRD measurement, the value of the peak position (2θ) is allowed to deviate by ±0.50°.
[0121] The composite compound obtained by combining the compounds shown in (H1) above is Li(FSI)(SN) 2 The melting point may be 63.4°C or around there. In addition, the composite compound obtained by combining the compounds shown in (H2) above is Li(FSI)(GN) 2 The melting point may be 89.3°C or close to that. In addition, the composite compound obtained by combining the compounds shown in (H3) above is Li(FSI)(ADN) 2 and the melting point may be 90.9°C or thereabouts.
[0122] That is, when it is desired to obtain a composite compound 117 having a high melting point, it is more preferable to use a composite compound obtained by combining the compounds shown in (H2) and (H3) above than a composite compound obtained by combining the compounds shown in (H1) above.
[0123] Next, the magnitude of the charge on the nitrogen atom of succinonitrile, glutaronitrile, and adiponitrile, which can be used in the first compound, was calculated. The nitrogen atom can form a coordinate bond with a lithium ion, and the strength of the coordinate bond between the lithium ion and the first compound can be determined and compared based on the magnitude of the charge on the nitrogen atom. Gaussian09 was used as the quantum chemistry calculation software for the calculation. After optimizing the ground state molecular structures of succinonitrile, glutaronitrile, and adiponitrile, the charge distribution within the molecule was analyzed to determine the magnitude of the charge.
[0124] First, ground-state structural optimization calculations were performed on succinonitrile, glutaronitrile, and adiponitrile, which can be used for the first compound. Density functional theory (DFT) was used for the structural optimization calculations. The total energy in DFT is expressed as the sum of potential energy, interelectronic electrostatic energy, and exchange-correlation energy, which includes electron kinetic energy and complex electron-electron interactions. DFT also approximates the exchange-correlation interaction with a single-electron potential functional (a function of a function) expressed in terms of electron density, allowing for fast and highly accurate calculations. In this study, the mixed functional B3LYP was used to define the weights of each parameter related to the exchange and correlation energy. The 6-311G basis set (a triple-split valence basis set using three contraction functions for each valence orbital) was applied to all atoms. With the above-mentioned basis functions, for example, the 1s to 3s orbitals are considered for a hydrogen atom, and the 1s to 4s and 2p to 4p orbitals are considered for a carbon atom. Furthermore, to improve the calculation accuracy, a p-function is added to the hydrogen atom and a d-function is added to atoms other than the hydrogen atom as a polarization basis set.
[0125] The charge distribution was analyzed by fitting the electrostatic potential to charge using points based on the scheme of the Merz-Singh-Kollmans (MK) method. The calculation conditions are summarized in Table 1 below.
[0126]
[0127] Figure 48A shows the structural formula of succinonitrile and the magnitude of the charge on the nitrogen atom of succinonitrile. The charge on each nitrogen atom of succinonitrile is -0.42. Figure 48B shows the structural formula of glutaronitrile and the magnitude of the charge on each nitrogen atom of glutaronitrile. The charge on each nitrogen atom of glutaronitrile is -0.44. Figure 48C shows the structural formula of adiponitrile and the magnitude of the charge on each nitrogen atom of adiponitrile. The charge on each nitrogen atom of adiponitrile is -0.46.
[0128] It is speculated that the longer the carbon chain of succinonitrile, glutaronitrile, and adiponitrile, the stronger the charge on the nitrogen atom and the stronger the coordination bond with the lithium ion. Therefore, it is speculated that the coordination bond between adiponitrile and lithium ion is strong.
[0129] Next, an example of calculation results regarding the stable structure of a complex compound is shown in Figure 49. The calculation was performed using the calculation conditions shown in Table 2 below.
[0130]
[0131] Figure 49A shows an example of a stable structure of a complex compound containing succinonitrile and lithium bis(fluorosulfonyl)imide. It can be seen that the complex compound shown in Figure 49A contains succinonitrile 182, lithium ion 180, and (fluorosulfonyl)imide ion 181.
[0132] In addition, in the case of a stable structure, the composite compound has a partial structure in which a cyano group is coordinately bonded to a lithium ion, as shown in the following general formula (G2).
[0133]
[0134] In the general formula (G2), R represents a hydrocarbon having 1 to 5 carbon atoms. Preferably, in the general formula (G2), R represents a hydrocarbon having 2 to 4 carbon atoms.
[0135] In the case of the stable structure shown in FIG. 49A, the composite compound has a partial structure in which succinonitrile is coordinately bonded to a lithium ion, as shown in (H4) below.
[0136]
[0137] Figure 49B shows an example of a stable structure of a complex compound of glutaronitrile and lithium bis(fluorosulfonyl)imide. It can be seen that the complex compound shown in Figure 49B has glutaronitrile 187, lithium ion 185, and bis(fluorosulfonyl)imide ion 186. That is, in the case of the stable structure of Figure 49B, the complex compound has a partial structure in which glutaronitrile is coordinately bonded to a lithium ion.
[0138] Figure 49C shows an example of a stable structure of a complex compound of adiponitrile and lithium bis(fluorosulfonyl)imide. It can be seen that the complex compound shown in Figure 49C has adiponitrile 192, lithium ion 190, and bis(fluorosulfonyl)imide ion 191. That is, in the case of the stable structure of Figure 49C, the complex compound has a partial structure in which adiponitrile is coordinately bonded to a lithium ion.
[0139] Next, an example of the configuration of an all-solid-state secondary battery using the composite compound 117 as an electrolyte will be described. Fig. 2B shows a cross-sectional view of a secondary battery 150 that serves as an all-solid-state secondary battery. The secondary battery 150 does not include a separator, uses the composite compound 117 as an electrolyte, uses a positive electrode active material 115 at least partially covered with a barrier layer 116, or the like, as a positive electrode active material, and uses a first negative electrode active material 125 and a second negative electrode active material 129, or the like, as negative electrode active materials.
[0140] The composite compound 117 is mixed with the positive electrode active material 115 and the like to obtain the positive electrode side structure of the secondary battery 150. The composite compound 117 is arranged so as to fill the spaces between the positive electrode active material particles. The composite compound 117 is mixed with the first negative electrode active material 125, the second negative electrode active material 129 and the like to obtain the negative electrode side structure of the secondary battery 150.
[0141] Although FIG. 2B shows an all-solid-state secondary battery that does not include a separator, it may also include a separator.
[0142] The content of this embodiment mode can be combined with the content of other embodiment modes as appropriate.
[0143] (Embodiment 2) In this embodiment, a secondary battery according to one embodiment of the present invention will be described. The secondary battery includes at least a positive electrode, a negative electrode, an electrolyte, and an outer casing. A separator may be provided between the positive electrode and the negative electrode. In the positive electrode, the positive electrode active material layer preferably includes a positive electrode active material and a composite compound, and more preferably, the composite compound is positioned so as to cover the surface of the positive electrode active material. The composite compound preferably has crystallinity, for example, molecular crystals. The molecular crystal preferably has high ionic conductivity and can be used as an electrolyte. In this case, the composite compound can be called a molecular crystal electrolyte.
[0144] An example of a method for manufacturing a secondary battery of one embodiment of the present invention will be described with reference to FIGS.
[0145] [Method 1 for Fabricating a Positive Electrode] A method for fabricating a positive electrode according to one embodiment of the present invention will be described with reference to FIGS. 3 and 4. The positive electrode active material layer preferably includes the positive electrode active material composite described in Embodiment 3 or the positive electrode active material described in Embodiment 4, and may further include a composite compound, a conductive material, and the like. The composite compound preferably functions as a binder that binds together a plurality of positive electrode active material composites or a plurality of positive electrode active materials. Furthermore, the composite compound preferably allows lithium ions to pass through.
[0146] In step S91 of FIG. 3A, a first compound 15 is prepared, and in step S92, a second compound 16 is prepared. Next, in step S93, the first compound 15 and the second compound 16 are mixed while being heated. Mixing after heating is also possible as long as the heated temperature can be maintained. The heating temperature in step S93 is preferably a temperature or higher (e.g., a melting point or higher) at which the mixture of the first compound 15 and the second compound 16 is completely melted. The heating in step S93 may be multi-stage heating. After the heating and mixing in step S93, the mixture is cooled to room temperature, and a composite compound 117 is obtained in step S94. The composite compound 117 has molecular crystals and can cover the positive electrode active material, etc., as the composite compound 117 having a crystalline structure.
[0147] As the first compound 15, a nitrile solvent can be used, for example, any one or more of acetonitrile, succinonitrile, glutaronitrile, and adiponitrile can be used.
[0148] The second compound 16 is lithium bis(fluorosulfonyl)imide (Li(FSO 2 ) 2 N, abbreviated as LiFSI), lithium bis(trifluoromethanesulfonyl)imide (Li(CF 3 SO 2 ) 2 N, abbreviated as LiTFSI), and lithium bis(pentafluoroethanesulfonyl)imide (Li(C2 F 5 SO 2 ) 2 N, abbreviated as LiBETI).
[0149] The composite compound 117 preferably functions as a binder that binds together a plurality of positive electrode active material composites or a plurality of positive electrode active materials. Furthermore, the composite compound 117 preferably allows lithium ions to pass through. Furthermore, the composite compound 117 preferably has crystallinity, and more preferably is a molecular crystal having the first compound 15 and the second compound 16.
[0150] 3B, a positive electrode active material 115 is prepared. As the positive electrode active material 115, the positive electrode active material composite described in Embodiment 3 or the positive electrode active material described in Embodiment 4 may be used.
[0151] In step S96 of Fig. 3B, a composite compound 117 is prepared. For example, the composite compound 117 prepared in Fig. 3A can be used. Instead of preparing the composite compound 117 in step S96, the first compound 15 in step S91 of Fig. 3A and the second compound 16 in step S92 may be prepared as they are.
[0152] Next, in step S97, positive electrode active material 115 and composite compound 117 are mixed while being heated, and in step S98, mixture 140 is obtained. Mixture 140 may be referred to as positive electrode slurry. In step S97, positive electrode active material 115, first compound 15, and second compound 16 from step S92 may also be mixed while being heated, and mixture 140 may be obtained in step S98.
[0153] If the temperature of the heated state in step S97 can be maintained, the mixture may be mixed after heating. In step S99, the mixture is heated and applied to a current collector. After cooling in step S100, the positive electrode 101 is obtained in step S101. In the positive electrode 101, the composite compound 117 is preferably solid.
[0154] Step S97 may be a step of heating the positive electrode active material 115, the first compound 15, and the second compound 16 while mixing them.
[0155] Furthermore, in step S97, a conductive material may be added in addition to the positive electrode active material 115 and the composite compound 117. As the conductive material, for example, one or more materials selected from carbon black such as acetylene black or furnace black, graphite such as artificial graphite or natural graphite, carbon fiber such as carbon nanofiber or carbon nanotube, graphene, and a graphene compound can be used.
[0156] In this specification and the like, graphene includes single-layer graphene and multi-layer graphene (also referred to as multi-graphene). In addition, in this specification and the like, graphene compounds include graphene oxide, multi-layer graphene oxide, reduced graphene oxide, reduced multi-layer graphene oxide, etc. Graphene refers to a substance that contains carbon, has a shape such as a plate or sheet, and has a two-dimensional structure formed by six-membered carbon rings. Graphene may also be referred to as a carbon sheet. Graphene or graphene compounds preferably have a bent shape. Graphene compounds preferably have a functional group. Graphene or graphene compounds may be rolled into a cylindrical shape.
[0157] The heating in steps S97 and S99 is preferably performed at a temperature equal to or higher than the temperature at which the composite compound 117 is completely melted. For example, the composite compound 117 may be Li(FSI)(SN) 2 When using a compound 117, it is preferable to perform heating at a temperature of 60° C. or higher and 100° C. or lower, preferably 65° C. or higher and 80° C. or lower. However, the heating temperature in step S97 does not need to be equal to the heating temperature in step S99, and it is preferable that the heating temperature in step S97 is higher than the heating temperature in step S99. It is preferable that the composite compound 117 is a liquid in steps S97 and S99.
[0158] The positive electrode current collector can be made of a highly conductive material, such as a metal such as stainless steel, gold, platinum, aluminum, or titanium, or an alloy thereof. It is preferable that the material used for the positive electrode current collector does not leach at the potential of the positive electrode. The positive electrode current collector can be made of an aluminum alloy containing an element that improves heat resistance, such as silicon, titanium, neodymium, scandium, or molybdenum. The positive electrode current collector can be in any suitable shape, such as a foil, plate, sheet, mesh, punched metal, or expanded metal. The positive electrode current collector preferably has a thickness of 5 μm or more and 30 μm or less.
[0159] [Positive Electrode Fabrication Method 2] Next, a method for carrying out the present invention, which is different from the positive electrode fabrication method 1, will be described.
[0160] In step S102 of FIG. 4A, the binder 111 is prepared, and in step S103, the dispersion medium 120 is prepared.
[0161] The binder 111 may be, for example, one or more selected from the group consisting of polystyrene, polymethyl acrylate, polymethyl methacrylate (polymethyl methacrylate, PMMA), sodium polyacrylate, polyvinyl alcohol (PVA), polyethylene oxide (PEO), polypropylene oxide, polyimide, polyvinyl chloride, polytetrafluoroethylene, polyethylene, polypropylene, polyisobutylene, polyethylene terephthalate, nylon, polyvinylidene fluoride (PVDF), polyacrylonitrile (PAN), ethylene propylene diene polymer, polyvinyl acetate, and nitrocellulose. The lithium ion conductivity of the material used for the binder is preferably lower than that of the composite compound 117.
[0162] The dispersion medium 120 may be one or more selected from the group consisting of water, methanol, ethanol, acetone, tetrahydrofuran (THF), dimethylformamide (DMF), N-methylpyrrolidone (NMP), and dimethyl sulfoxide (DMSO), and may be referred to as a mixed liquid when two or more of these are used. A suitable combination of the binder 111 and the dispersion medium 120 is the combination of polyvinylidene fluoride (PVDF) and N-methylpyrrolidone (NMP).
[0163] Next, in step S104, the binder 111 and the dispersion medium 120 are mixed to obtain a mixture in step S105. To distinguish this mixture from other mixtures, it is referred to as a binder mixture 1001. For example, a propeller mixer, a planetary rotation mixer, or a thin film swirl mixer can be used as a mixing method. It is desirable that the binder mixture 1001 be in a state in which the binder 111 is well dispersed in the dispersion medium 120.
[0164] 4B, a binder mixture 1001 is prepared in step S111, and a conductive material 1002 is prepared in step S112. In order to perform the thickening process in a later step, the amount of binder mixture 1001 prepared in step S111 can be an amount smaller than the total amount required to form the positive electrode active material layer, and can be a mixed amount suitable for the thickening process. In this case, the shortfall in the binder mixture 1001 can be added in a step after the thickening process. Note that the thickening process refers to the kneading of a highly viscous mixture.
[0165] The conductive material 1002 may be, for example, one or more selected from carbon black such as acetylene black or furnace black, graphite such as artificial graphite or natural graphite, carbon fiber such as carbon nanofiber or carbon nanotube, graphene, and graphene compounds.
[0166] Next, in step S113, the binder mixture 1001 and the conductive material 1002 are mixed, and in step S121, a mixture 1010 is obtained. As a mixing method, for example, a propeller type mixer, a planetary rotation type mixer, or a thin film swirl type mixer can be used.
[0167] Next, in step S122 of FIG. 4B, the positive electrode active material 115 is prepared.
[0168] Next, in step S123, mixture 1010 and positive electrode active material 115 are mixed to obtain mixture 1020 in step S131. Mixing methods that can be used include, for example, a propeller mixer, a planetary rotation mixer, or a thin film swirl mixer. In step S123, if the viscosity is appropriately adjusted, thick kneading is possible, and thick kneading can break up agglomerations of powders such as the positive electrode active material.
[0169] Next, in step S132, a binder mixture 1001 is prepared, and in step S133, a dispersion medium 1003 is prepared. If, in step S111, an amount of binder mixture 1001 prepared is less than the total amount necessary to form the positive electrode active material layer, the shortage of binder mixture 1001 can be added in step S132. When adjusting the dispersion medium for binder mixture 1001, a dispersion medium similar to that in step S102 of FIG. 4A can be prepared as dispersion medium 1003. It is desirable to adjust the amount of dispersion medium 1003 to be prepared so that the viscosity is appropriate for application in a later step. Note that, if the entire amount of binder mixture 1001 necessary to form the positive electrode active material layer is prepared in step S111, it is not necessary to prepare binder mixture 1001 in step S132. In other words, if the entire amount of binder mixture 1001 necessary to form the positive electrode active material layer is prepared in step S111, steps S132, S133, and S134 can be omitted.
[0170] Next, in step S134, the mixture 1020 from step S131, the binder mixture 1001 prepared in step S132, and the dispersion medium 1003 prepared in step S133 are mixed together, and in step S135, a mixture 1030 is obtained. The mixture 1030 may be referred to as a positive electrode slurry.
[0171] Next, in step S136, the mixture 1030 is applied to a positive electrode current collector. Highly conductive materials, such as metals such as stainless steel, gold, platinum, aluminum, and titanium, and alloys thereof, can be used for the positive electrode current collector. It is preferable that the material used for the positive electrode current collector does not dissolve at the potential of the positive electrode. The application method in step S136 can be a slot die method, a gravure method, a blade method, or a combination thereof. A continuous coater or the like can also be used for application. Following step S136, in step S137, the mixture 1030 applied to the positive electrode current collector is dried. Examples of drying methods include batch methods using a hot plate, a drying oven, a forced air drying oven, and a vacuum drying oven, as well as continuous methods combining a continuous coater with hot air drying and infrared drying. After drying, a coated electrode 1040 is obtained in step S140.
[0172] Next, in step S141 of FIG. 4B, the complex compound 117 of step S112 of FIG. 3A is prepared.
[0173] Next, in step S142 of FIG. 4B , the coated electrode 1040 and the composite compound 117 of step S140 are heated, and the composite compound 117 is injected into the voids of the coated electrode 1040. The heating temperature is preferably equal to or higher than the temperature at which the composite compound 117 completely melts. The injection method can be one or more selected from a slot die method, a gravure method, a blade method, a dropping method such as ODF (One Drop Filling), a flat plate press method, a roll press method, and a combination thereof. Injection in a reduced pressure environment is preferable because it allows the composite compound 117 to effectively infiltrate the voids of the coated electrode 1040. For example, Li(FSI)(SN)2 When using the above, the heating temperature is 60°C or higher and 100°C or lower, preferably 65°C or higher and 80°C or lower.
[0174] The positive electrode active material is fixed to the positive electrode current collector or other positive electrode active materials by the binder mixed in advance. Injecting the liquid composite compound 117 in this state allows the composite compound 117 to efficiently infiltrate the voids. Because the composite compound 117 solidifies at room temperature, it can also function as a binder. It is preferable that the composite compound 117 has high ionic conductivity. This configuration allows the proportion of binder in conventional positive electrodes to be reduced and the proportion of positive electrode active material to be increased. Furthermore, a pressing process is sometimes performed on the coated electrode when forming the positive electrode, but the pressing pressure can be reduced by performing this injection in a reduced-pressure environment. Furthermore, performing the injection in a reduced-pressure environment can eliminate the pressing process.
[0175] Through the above steps, the positive electrode 101 of one embodiment of the present invention illustrated in FIG. 4B can be manufactured (Step S143).
[0176] [Method for Producing Negative Electrode] The negative electrode can be produced in the same manner as the method for producing the positive electrode 101 shown in Figures 3 and 4. When producing the negative electrode 102 using the production method shown in Figures 3 and 4, a negative electrode active material is prepared instead of the positive electrode active material 115 prepared in step S121 of Figure 3B. Furthermore, a negative electrode active material is prepared instead of the positive electrode active material 115 prepared in step S122 of Figure 4B.
[0177] As the negative electrode active material, for example, an alloy-based material, a carbon-based material, or a mixture thereof can be used.
[0178] As the negative electrode active material, an element capable of undergoing a charge-discharge reaction by alloying / de-alloying with lithium can be used. For example, a material containing at least one of silicon, tin, gallium, aluminum, germanium, lead, antimony, bismuth, silver, zinc, cadmium, indium, etc. can be used. These elements have a larger capacity than carbon, and silicon in particular has a high theoretical capacity of 4200 mAh / g. For this reason, it is preferable to use silicon as the negative electrode active material. Alternatively, a composite compound containing these elements may be used as the negative electrode active material. For example, SiO, Mg 2 Si, Mg 2 Ge, SnO, SnO 2 , Mg 2 Sn, SnS 2 , V 2 Sn 3 , FeSn 2 , CoSn 2 , Ni 3 Sn 2 , Cu 6 Sn 5 , Ag 3 Sn, Ag 3 Sb, Ni 2 MnSb, CeSb 3 , LaSn 3 , La 3 Co 2 Sn 7 , CoSb 3 , InSb, SbSn, etc. Here, elements that can undergo charge-discharge reactions by alloying / dealloying reactions with lithium, and composite compounds containing such elements, are sometimes referred to as alloy-based materials.
[0179] In this specification and the like, SiO refers to, for example, silicon monoxide. Alternatively, SiO refers to SiO x Here, x preferably has a value of 1 or close to 1. For example, x is preferably 0.2 or more and 1.5 or less, and more preferably 0.3 or more and 1.2 or less.
[0180] The negative electrode active material may be a carbon-based material such as graphite, easily graphitizable carbon (soft carbon), hardly graphitizable carbon (hard carbon), carbon nanotubes, graphene, or carbon black.
[0181] Examples of graphite include artificial graphite and natural graphite. Examples of artificial graphite include mesocarbon microbeads (MCMB), coke-based artificial graphite, and pitch-based artificial graphite. As the artificial graphite, spherical graphite having a spherical shape can be used. For example, MCMB may have a spherical shape and is preferred. Furthermore, it is relatively easy to reduce the surface area of MCMB, and therefore it is preferred. Examples of natural graphite include flake graphite and spherical natural graphite.
[0182] When lithium ions are intercalated into graphite, the graphite exhibits a potential as low as that of metallic lithium. This allows lithium-ion secondary batteries using graphite to exhibit high operating voltages. Graphite is also preferred because it has advantages such as a relatively high capacity per unit volume, relatively small volume expansion, low cost, and higher safety compared to metallic lithium.
[0183] Titanium dioxide (TiO 2 ), lithium titanium oxide (Li 4 Ti 5 O 12 ), niobium pentoxide (Nb 2 O 5 ), tungsten oxide (WO 2 ), molybdenum oxide (MoO 2 ) and other oxides can be used.
[0184] In addition, as the negative electrode active material, a lithium-graphite intercalation compound (Li x C 6 ), SiC, etc. can be used.
[0185] In addition, as the negative electrode active material, a nitride of lithium and a transition metal, Li 3 Li with N-type structure 3−x M x N (M=Co, Ni, Cu) can be used. For example, Li2.6 Co 0.4 N 3 has a large discharge capacity (900 mAh / g, 1890 mAh / cm 3 ) and is preferred.
[0186] When a nitride of lithium and a transition metal is used, lithium ions are contained in the negative electrode active material, so V, which does not contain lithium ions, is used as the positive electrode active material. 2 O 5 , Cr 3 O 8 It is preferable that the material can be combined with a material such as the above. Even when a material containing lithium ions is used as the positive electrode active material, it is possible to use a nitride of lithium and a transition metal as the negative electrode active material by first desorbing the lithium ions contained in the positive electrode active material.
[0187] Furthermore, a material that undergoes a conversion reaction can also be used as the negative electrode active material. For example, a transition metal oxide that does not form an alloy with lithium, such as cobalt oxide (CoO), nickel oxide (NiO), or iron oxide (FeO), can be used as the negative electrode active material. Further examples of materials that undergo a conversion reaction include Fe 2 O 3 ,CuO,Cu 2 O, RuO 2 , Cr 2 O 3 oxides such as CoS 0.89 , sulfides such as NiS and CuS, Zn 3 N 2 , Cu 3 N or Ge 3 N 4 Nitrides such as NiP 2 , FeP 2 , or CoP 3 Phosphides such as FeF 3 , or BiF 3 This also occurs with fluorides such as
[0188] The conductive material and binder that can be contained in the negative electrode active material layer can be the same as the conductive material and binder that can be contained in the positive electrode active material layer.
[0189] The negative electrode current collector may be made of copper or the like in addition to the same materials as the positive electrode current collector. It is preferable that the negative electrode current collector be made of a material that does not alloy with carrier ions such as lithium.
[0190] A negative electrode can be fabricated according to FIGS. 3A and 3B using the negative electrode active materials and the like described above. In this case, negative electrode 102 can be obtained in step S130 of FIG. 3B. Alternatively, a negative electrode can be fabricated according to FIGS. 4A and 4B using the negative electrode active materials and the like described above. In this case, negative electrode 102 can be obtained in step S143 of FIG. 4B.
[0191] [Secondary Battery Manufacturing Method 1] A method for manufacturing a secondary battery of one embodiment of the present invention will be described with reference to FIGS. 5A and 5B.
[0192] In FIG. 5A, positive electrode 101 is prepared in step S141, negative electrode 102 is prepared in step S142, separator 110 is prepared in step S143, and exterior body 230 is prepared in step S144.
[0193] The separator can be made of, for example, cellulose-containing fibers such as paper, nonwoven fabric, glass fiber, ceramics, or synthetic fibers such as nylon (polyamide), vinylon (polyvinyl alcohol-based fiber), polyester, polyimide, acrylic, polyolefin, or polyurethane.
[0194] The separator may have a multilayer structure. For example, an organic film such as polypropylene or polyethylene may be coated with a ceramic material, a fluorine-based material, a polyamide material, or a mixture of these. Examples of ceramic materials include aluminum oxide particles and silicon oxide particles. Examples of fluorine-based materials include PVDF and polytetrafluoroethylene. Examples of polyamide materials include nylon and aramid (meta-aramid and para-aramid).
[0195] Coating the above materials with ceramic materials improves oxidation resistance, suppressing separator degradation during high-voltage charging and improving the reliability of secondary batteries. Coating with fluorine-based materials also improves adhesion between the separator and electrodes, improving output characteristics. Coating with polyamide-based materials, especially aramid, improves heat resistance, improving the safety of secondary batteries.
[0196] For example, both sides of a polypropylene film may be coated with a mixed material of aluminum oxide and aramid, or the surface of the polypropylene film that comes into contact with the positive electrode may be coated with a mixed material of aluminum oxide and aramid, and the surface that comes into contact with the negative electrode may be coated with a fluorine-based material.
[0197] The exterior can be made of a metal material such as aluminum or a resin material. Alternatively, a film-like exterior can be used. Examples of films that can be used include a three-layer structure in which a thin, flexible metal film made of aluminum, stainless steel, copper, nickel, or the like is provided on a film made of a material such as polyethylene, polypropylene, polycarbonate, ionomer, or polyamide, and an insulating synthetic resin film made of polyamide resin, polyester resin, or the like is further provided on the thin metal film as the exterior surface of the exterior.
[0198] Next, in step S145, the positive electrode 101, the negative electrode 102, the separator 110, and the exterior body 230 are assembled. The separator 110 is disposed between the positive electrode 101 and the negative electrode 102. The separator may be processed into a bag shape and disposed so as to encase either the positive electrode 101 or the negative electrode 102. Next, the positive electrode 101, the negative electrode 102, and the separator 110 are disposed inside the exterior body 230. At this time, it is desirable that the exterior body 230 has an opening for injecting the electrolyte. Note that electrode terminals such as leads may be provided as appropriate depending on the shape of the battery to be fabricated.
[0199] Next, in step S146, the electrolyte 240 is prepared.
[0200] An electrolytic solution having a solvent and an electrolyte dissolved in the solvent can be used as one form of the electrolyte 240. The solvent for the electrolytic solution is preferably an aprotic organic solvent, and for example, one or more selected from ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate, chloroethylene carbonate, vinylene carbonate, γ-butyrolactone, γ-valerolactone, dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), methyl formate, methyl acetate, ethyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, 1,3-dioxane, 1,4-dioxane, dimethoxyethane (DME), dimethyl sulfoxide, diethyl ether, methyl diglyme, acetonitrile, benzonitrile, tetrahydrofuran, sulfolane, and sultone can be used.
[0201] Furthermore, by using one or more flame-retardant and non-volatile ionic liquids (room-temperature molten salts) as the solvent for the electrolyte, it is possible to prevent the secondary battery from exploding or catching fire even if the internal temperature of the secondary battery rises due to an internal short circuit or overcharging. The ionic liquid is composed of a cation and an anion, and includes an organic cation and an anion. Examples of organic cations used in the electrolyte include aliphatic onium cations such as quaternary ammonium cations, tertiary sulfonium cations, and quaternary phosphonium cations, and aromatic cations such as imidazolium cations and pyridinium cations. Examples of anions used in the electrolyte include monovalent amide anions, monovalent methide anions, fluorosulfonate anions, perfluoroalkylsulfonate anions, tetrafluoroborate anions, perfluoroalkylborate anions, hexafluorophosphate anions, and perfluoroalkylphosphate anions.
[0202] The electrolyte to be dissolved in the solvent is, for example, LiPF 6 , LiClO 4 , LiAsF 6 , LiBF 4 , LiAlCl 4, LiSCN, LiBr, LiI, Li 2 SO 4 , Li 2 B 10 Cl 10 , Li 2 B 12 Cl 12 , LiCF 3 SO 3 , LiC 4 F 9 SO 3 , LiC(CF 3 SO 2 ) 3 , LiC(C 2 F 5 SO 2 ) 3 , LiN(CF 3 SO 2 ) 2 , LiN(C 4 F 9 SO 2 ) (CF 3 SO 2 ), LiN(C 2 F 5 SO 2 ) 2 , and lithium bis(oxalato)borate (Li(C) 2 O 4 ) 2 One or more lithium salts selected from the group consisting of LiBCO, LiBOB, LiBOB, and the like can be used.
[0203] It is preferable to use a highly purified electrolyte solution that contains little granular dust or elements other than the constituent elements of the electrolyte solution (hereinafter simply referred to as "impurities"). Specifically, it is preferable to set the weight ratio of impurities to the electrolyte solution to 1% or less, preferably 0.1% or less, and more preferably 0.01% or less.
[0204] The electrolyte solution may also contain one or more additives selected from vinylene carbonate, propane sultone (PS), tert-butylbenzene (TBB), fluoroethylene carbonate (FEC), lithium bis(oxalate)borate (LiBOB), and dinitrile composite compounds such as succinonitrile and adiponitrile. The concentration of the additive may be, for example, 0.1 wt % to 5 wt % relative to the solvent in which the electrolyte is dissolved.
[0205] Alternatively, a polymer gel electrolyte may be used in which a polymer is swollen with an electrolytic solution.
[0206] The use of a polymer gel electrolyte improves safety against leakage, etc. It also enables the secondary battery to be made thinner and lighter.
[0207] Examples of polymers that can be gelled include silicone gel, acrylic gel, acrylonitrile gel, polyethylene oxide gel, polypropylene oxide gel, and fluorine-based polymer gel. For example, polymers having a polyalkylene oxide structure such as polyethylene oxide (PEO), PVDF, polyacrylonitrile, and copolymers containing these can be used. For example, PVDF-HFP, a copolymer of PVDF and hexafluoropropylene (HFP), can be used. The formed polymer may also have a porous shape.
[0208] Next, in step S147, electrolyte 240 is poured from the opening of exterior body 230. Next, in step S148, the opening of exterior body 230 is sealed. Note that the pouring in step S147 and the sealing in step S148 may be performed in a reduced pressure atmosphere.
[0209] Through the above steps, the secondary battery 250 can be fabricated in step S149.
[0210] Secondary Battery Fabrication Method 2 Next, a method for carrying out the present invention, which is different from Secondary Battery Fabrication Method 1, will be described.
[0211] 5B, the positive electrode 101 is prepared, and the composite compound 117 is prepared in step S142. As the positive electrode 101, it is preferable to use the positive electrode 101 fabricated by the fabrication method of FIG.
[0212] Next, in step S143, the composite compound 117 is heated to a molten state and applied onto the active material layer of the positive electrode 101. The application method can be one or more selected from a slot die method, a gravure method, a blade method, and a combination thereof. A continuous coater or the like may also be used for application. Step S143 allows a layer containing the composite compound 117 to be formed on the positive electrode 101. The layer containing the composite compound 117 functions as a separator that prevents direct contact between the positive electrode 101 and the negative electrode 102, and as a solid electrolyte that can conduct lithium ions between the positive electrode 101 and the negative electrode 102.
[0213] Next, in step S144, the negative electrode 102 is prepared. It is preferable to use the negative electrode 102 fabricated according to the above-described method for fabricating a negative electrode shown in FIG.
[0214] Next, in step S145, heating and bonding are performed. The negative electrode 102 is placed on the structure having a layer of the composite compound 117 on the positive electrode 101 produced in step S143, and they are bonded together by heating. The heating in step S145 is preferably performed at a temperature equal to or lower than the temperature at which the composite compound 117 completely melts. That is, the heating in step S145 is preferably performed at a temperature lower than that in step S143. For example, Li(FSI)(SN) 2 When using the above, the heating temperature can be set to 55°C or higher and 65°C or lower.
[0215] Next, in step S146, the exterior body 230 is prepared.
[0216] Next, in step S147, the laminated positive electrode 101, negative electrode 102, and composite compound 117 are assembled with exterior body 230. Depending on the shape of the battery to be manufactured, electrode terminals such as leads may be provided as appropriate.
[0217] Next, in step S148, the exterior body 230 is sealed. The sealing is preferably performed under a reduced pressure atmosphere. Furthermore, during the sealing, the exterior body 230 containing the positive electrode 101, the negative electrode 102, and the composite compound 117 is preferably heated and pressed from the outside, since this reduces voids inside the positive electrode, the negative electrode, or the exterior body.
[0218] Instead of the composite compound 117 prepared in step S142, a solid electrolyte having an inorganic material such as a sulfide or oxide, or a solid electrolyte having a polymer material such as a PEO (polyethylene oxide) can be used as the electrolyte.
[0219] Through the above steps, the secondary battery 250 can be fabricated in step S149.
[0220] As described above, the secondary battery fabricated by secondary battery fabrication method 2 can be called an all-solid-state secondary battery. The all-solid-state secondary battery is a lithium-ion secondary battery that is highly safe and has excellent characteristics.
[0221] The contents described in this embodiment can be combined with the contents described in other embodiments.
[0222] Embodiment 3 In this embodiment, a positive electrode active material composite that can be used for the positive electrode active material 115 of one embodiment of the present invention, a manufacturing method thereof, a positive electrode, and a manufacturing method thereof will be described.
[0223] The positive electrode includes a positive electrode active material layer and a positive electrode current collector. The positive electrode active material layer includes a positive electrode active material composite 100z having a first material 100x that functions as a positive electrode active material and a second material 100y that covers at least a portion of the first material 100x. The second material 100y can function as the barrier layer 116 described in Embodiment 1 and the like. The barrier layer may also be referred to as a coating layer. The positive electrode active material layer may further include a conductive material and a binder. The binder may include a complex compound. When the binder includes a complex compound, the complex compound 117 can be disposed outside the second material 100y.
[0224] The positive electrode active material composite 100z is obtained by a composite process using at least a first material 100x and a second material 100y. The second material 100y may be an active material capable of absorbing and releasing lithium. The composite process may be one or more of the following: composite processes using mechanical energy, such as mechanochemical processes, mechanofusion processes, and ball milling processes; composite processes using liquid-phase reactions, such as coprecipitation processes, hydrothermal processes, and sol-gel processes; and composite processes using gas-phase reactions, such as barrel sputtering processes, atomic layer deposition (ALD), vapor deposition processes, and chemical vapor deposition (CVD). In this specification, the composite process is also referred to as a surface coating process or a coating process.
[0225] Furthermore, it is preferable to perform a heat treatment after the composite formation process. When the heat treatment is performed after the composite formation process, the second material 100y, which covers at least a portion of the first material 100x that functions as a positive electrode active material, sinters or melts and spreads. Therefore, it is expected that the effect of reducing the number of points of direct contact between the first material 100x and the electrolyte can be achieved. However, if the temperature of the heat treatment after the composite formation process is too high, the elements contained in the second material 100y may diffuse more than necessary into the first material 100x, which may reduce the charge / discharge capacity of the first material 100x as an active material and may reduce the effectiveness of the second material 100y as a barrier layer. Therefore, when performing the heat treatment after the composite formation process, it is recommended to appropriately set the heating temperature, heating time, and heating atmosphere.
[0226] [Positive Electrode Active Material] As the first material 100x, LiMO having a layered rock salt crystal structure 2 (M1 is one or more selected from Fe, Ni, Co, Mn, and Al) can be used as the first material 100x. 2A composite oxide represented by the formula (I) can be used in which an additive element X is added. The additive element X contained in the first material 100x is preferably one or more selected from nickel, cobalt, magnesium, calcium, chlorine, fluorine, aluminum, manganese, titanium, zirconium, yttrium, vanadium, iron, chromium, niobium, lanthanum, hafnium, zinc, silicon, sulfur, phosphorus, boron, and arsenic. These elements may further stabilize the crystal structure of the first material 100x. To further stabilize the crystal structure, the additive element X should be located in the surface layer of the positive electrode active material. That is, a region containing the additive element X is located in the surface layer. The region containing the additive element X located in the surface layer can also function as a barrier layer 116. Furthermore, the barrier layer 116 can have a region containing the additive element X and a second material 100y located outside of that region.
[0227] The first material 100x doped with the additive element X in this manner can include lithium cobalt oxide doped with magnesium and fluorine, lithium cobalt oxide doped with magnesium, fluorine, aluminum, and nickel, lithium cobalt oxide doped with magnesium, fluorine, and titanium, lithium nickel-cobalt oxide doped with magnesium and fluorine, lithium cobalt-aluminate doped with magnesium and fluorine, nickel-cobalt-lithium aluminum oxide, nickel-cobalt-lithium aluminum oxide doped with magnesium and fluorine, and nickel-cobalt-lithium manganese oxide doped with magnesium and fluorine. The region containing the additive element can be used as the barrier layer 116. The transition metal ratio of the nickel-cobalt-lithium manganese oxide is preferably high, and for example, a material having a ratio of nickel:cobalt:manganese of 8:1:1 or thereabouts, or nickel:cobalt:manganese of 9:0.5:0.5 or thereabouts is preferred. Furthermore, the lithium nickel-cobalt-manganese oxide preferably contains calcium-added lithium nickel-cobalt-manganese oxide.
[0228] Also, as the first material 100x, LiMO2 Secondary particles of a composite oxide represented by the formula (where M1 is one or more selected from Fe, Ni, Co, Mn, and Al) coated with a metal oxide may also be used. The metal oxide may be an oxide of one or more metals selected from Al, Ti, Nb, Zr, La, and Li. For example, LiMO 2 A complex oxide (sometimes referred to as a metal oxide-coated complex oxide) in which secondary particles of a complex oxide represented by the formula (M1 is one or more selected from Fe, Ni, Co, Mn, and Al) are coated with aluminum oxide can be used as the first material 100x. For example, a metal oxide-coated complex oxide in which secondary particles of nickel-cobalt-lithium manganese oxide having a ratio of nickel:cobalt:manganese=8:1:1 or nickel:cobalt:manganese=9:0.5:0.5 are coated with aluminum oxide can be used. A region having a metal oxide such as aluminum oxide can be used as the barrier layer 116.
[0229] Here, the thickness of the region where the second material 100y functioning as a barrier layer is located is preferably small, for example, from 1 nm to 200 nm, more preferably from 1 nm to 100 nm.
[0230] The first material 100x can be formed by the method described in Embodiment 4 below.
[0231] The second material 100y is LiM2PO4 having an oxide and an olivine-type crystal structure. 4 (M2 is one or more selected from Fe, Ni, Co, and Mn). Many oxides have stable crystal structures, and examples of oxides include aluminum oxide, zirconium oxide, hafnium oxide, and niobium oxide. LiM2PO 4 Many of them have stable crystal structures, and LiMPO 4 As an example, LiFePO 4 , LiNiPO 4 , LiCoPO 4 , LiMnPO 4 , LiFe a Ni b P.O. 4, LiFe a Co b P.O. 4 , LiFe a Mn b P.O. 4 , LiNi a Co b P.O. 4 , LiNi a Mn b P.O. 4 (a+b is 1 or less, 0<a<1, 0<b<1), LiFe c Ni d Co e P.O. 4 , LiFe c Ni d Mn e P.O. 4 , LiNi c Co d Mn e P.O. 4 (c+d+e is 1 or less, 0<c<1, 0<d<1, 0<e<1), or LiFe f Ni g Co h Mn i P.O. 4 (f+g+h+i is 1 or less, 0<f<1, 0<g<1, 0<h<1, 0<i<1), etc.
[0232] Furthermore, when the second material 100y is in particulate form, the surface of the particles may have a carbon coating layer.
[0233] [Cathode Active Material Composite] In this embodiment, an example of a method for producing a cathode active material composite in which at least a portion of the particle surface of a particulate first material 100x that functions as a cathode active material is covered with a second material 100y is shown as cathode active material composite production method 1. A desirable form of the cathode active material composite is a structure in which at least a portion of the particle surface of the particulate first material 100x is covered with the second material 100y, and more preferably a structure in which substantially the entire particle surface of the particulate first material 100x is covered with the second material 100y. Here, "substantially covering the entire particle surface" means that the second material 100y is positioned to such an extent that the first material 100x and the electrolyte do not come into direct contact with each other.
[0234] Furthermore, a configuration in which almost the entire particle surface of the first material 100x is covered with the second material 100y after the composite process may have different charge / discharge characteristics than a configuration in which the second material 100y and the first material 100x are simply mixed.
[0235] When at least a portion, and preferably almost the entire particle surface, of the first material 100x that functions as a positive electrode active material is covered with the second material 100y, the area in which the first material 100x is in direct contact with the electrolyte is reduced, and therefore, even in a high-voltage charging state, it is possible to suppress the desorption of transition metal elements and / or oxygen from the first material 100x, and to suppress the decrease in capacity due to repeated charging and discharging.
[0236] Furthermore, when a material with a stable crystal structure is used for the second material 100y, the secondary battery of one embodiment of the present invention can achieve effects such as suppressing the desorption of transition metal elements and / or oxygen from the first material 100x even in a high-voltage charging state, improving stability at high temperatures, and improving fire resistance.
[0237] The first material 100x preferably includes lithium cobalt oxide doped with magnesium and / or fluorine, and lithium cobalt oxide doped with magnesium, fluorine, aluminum, and / or nickel. Magnesium, fluorine, and aluminum are characterized by their abundance in the surface layer of the positive electrode active material, while nickel is characterized by its widespread distribution throughout the positive electrode active material. The first material 100x preferably includes secondary particles of nickel-cobalt-manganese lithium oxide with a nickel:cobalt:manganese ratio of 8:1:1 or thereabouts, or a nickel:cobalt:manganese ratio of 9:0.5:0.5 or thereabouts. The positive electrode active material composite preferably includes a metal oxide-coated composite oxide, in which the first material 100x is coated with aluminum oxide, providing excellent stability during high-voltage charging. This further improves the durability and stability of the positive electrode active material during high-voltage charging. Furthermore, the use of the above-described positive electrode active material composite further improves the heat resistance and / or fire resistance of the secondary battery.
[0238] The positive electrode active material that has been subjected to initial heating, which will be described later, is particularly preferable as the first material 100x because it has significantly excellent high-voltage charge / discharge cycle characteristics.
[0239] In an embodiment, the positive electrode of the present invention may have a structure in which at least a portion of the surface of the positive electrode active material composite is covered with graphene or a graphene compound. Preferably, the positive electrode active material composite has a structure in which 80% or more of the surface of the positive electrode active material composite and / or an aggregate having the positive electrode active material composite is covered with graphene or a graphene compound.
[0240] [Method for Producing a Positive Electrode Active Material Composite] An example of a method for producing a positive electrode active material composite according to one embodiment of the present invention will be described with reference to Fig. 6. In the method for producing a positive electrode active material composite, a second material 100y and a first material 100x are subjected to a composite treatment using mechanical energy. However, the present invention should not be construed as being limited to the contents of this description.
[0241] In step S101 of FIG. 6A, a first material 100x is prepared, and in step S102, a second material 100y is prepared.
[0242] The first material 100x is LiMO prepared by the method shown in the fourth embodiment described later. 2(M1 is one or more selected from Fe, Ni, Co, Mn, and Al), to which an additive element X has been added, can be used. For example, lithium cobalt oxide to which magnesium and fluorine have been added, or lithium cobalt oxide to which magnesium, fluorine, aluminum, and nickel have been added, can be used. In particular, lithium cobalt oxide to which magnesium, fluorine, aluminum, and nickel have been added is preferably one that has undergone the initial heating process described in the fourth embodiment. Another example of the first material 100x is lithium nickel-cobalt-manganese oxide. Here, the transition metal ratio of the nickel-cobalt-manganese oxide is preferably a high nickel ratio, for example, nickel:cobalt:manganese = 8:1:1 or thereabouts, or nickel:cobalt:manganese = 9:0.5:0.5 or thereabouts. Another example of the first material 100x is a metal oxide-coated complex oxide in which secondary particles of nickel-cobalt-manganese lithium are coated with aluminum oxide. Here, it is preferable that the aluminum oxide is thin, and the film thickness of the aluminum oxide is, for example, 1 nm or more and 200 nm or less, more preferably 1 nm or more and 100 nm or less.
[0243] Again, the second material 100y is LiM2PO 4 (M2 is one or more selected from Fe, Ni, Co, and Mn). Alternatively, an oxide can be used as the second material 100y. Examples of the oxide include one or more selected from aluminum oxide, zirconium oxide, hafnium oxide, and niobium oxide. LiM2PO 4 The materials mentioned above as LiFePO 4 , LiMnPO 4 , LiFe a Mn b P.O. 4 (a+b is 1 or less, 0<a<1, 0<b<1), or LiFe a Ni b P.O. 4 (a+b is 1 or less, 0<a<1, 0<b<1) can be used. When the second material 100y is in a particulate form, the surface of the particle may have a carbon coating layer.
[0244] It is also possible to use a material that functions as a positive electrode active material as the second material 100y. In this case, as a combination of the first material 100x and the second material 100y, it is possible to select a combination that is less likely to produce a step in the charge / discharge curve, depending on the characteristics required of the secondary battery, or a combination that produces a step in the charge / discharge curve at a desired charging rate. The step in the charge / discharge curve is sometimes referred to as a plateau, and includes a region where stable output can be obtained.
[0245] Next, in step S103, the first material 100x and the second material 100y are combined. When combining using mechanical energy, the combining can be performed by a mechanochemical method. Alternatively, the combining can be performed by a mechanofusion method.
[0246] Furthermore, when performing the composite treatment using a ball mill in step S103, it is preferable to use zirconia balls as media, for example. Dry treatment is preferable for the ball mill treatment. When wet treatment is performed for the ball mill treatment, acetone can be used. When wet treatment is performed, it is recommended to use dehydrated acetone with a water content of 100 ppm or less, preferably 10 ppm or less.
[0247] By the compounding process in step S103, at least a part of the particle surface of the particulate first material 100x, preferably almost the entire particle surface, can be covered with the second material 100y.
[0248] Through the above steps, the positive electrode active material composite 100z of one embodiment of the present invention shown in FIG. 6A can be manufactured (Step S104).
[0249] Next, a manufacturing method of Fig. 6B that is different from Fig. 6A will be described. In Fig. 6B, the manufacturing method up to step S103 is the same as the manufacturing method shown in Fig. 6A, and after step S103, heat treatment is performed in step S104. The heating in step S104 is preferably performed in an oxygen-containing atmosphere at a temperature of 400°C to 950°C, preferably 450°C to 800°C, for 1 hour to 60 hours, preferably 2 hours to 20 hours.
[0250] Through the above steps, the positive electrode active material composite 100z of one embodiment of the present invention shown in FIG. 6B can be manufactured (Step S105).
[0251] In order to obtain a good coating state in the composite process, the ratio of the particle size of the second material 100y to the particle size of the first material 100x (particle size of the second material 100y / particle size of the first material 100x) is preferably 1 / 200 or more and 1 / 50 or less, and more preferably 1 / 200 or more and 1 / 100 or less. To adjust the particle size of the second material 100y, an atomization process as shown in FIG. 6C may be performed. The atomization process involves pulverization and classification via step S102a in FIG. 6C when preparing the second material 100y in step S102 of FIGS. 6A and 6B. The atomization process allows for the production of a second material 100y' with an adjusted particle size in step S102b.
[0252] [Calculations for the Positive Electrode Active Material Composite] As an example of the positive electrode active material composite, LiCoO having a layered rock salt structure was used as the first material. 2 and LiFePO with an olivine structure as the second material. 4 , LiCoO 2 , LiFe 0.5 Mn 0.5 P.O. 4 , or LiFe 0.5 Ni 0.5 P.O. 4 The structure of LiCoO was evaluated using density functional theory (DFT). 2 and LiFePO 4 and a structure in which LiCoO 2 and LiFe 0.5 Mn 0.5 P.O.4 or LiFe 0.5 Ni 0.5 P.O. 4 The structure in which and are bonded was optimized and evaluated using DFT. The main calculation conditions are shown in Table 3.
[0253]
[0254] LiCoO 2 and LiFePO 4 The initial state of the model used to calculate the structure in which LiCoO and LiCoO are bonded is shown in Figure 7A. 2 and LiFe 0.5 Mn 0.5 P.O. 4 or LiFe 0.5 Ni 0.5 P.O. 4 The initial state of the model used to calculate the structure in which LiFe and 0.5 Mn 0.5 P.O. 4 or LiFe 0.5 Ni 0.5 P.O. 4 LiFe 0.5 M 0.5 P.O. 4 It is written as LiFePO 4 , LiFe 0.5 Mn 0.5 P.O. 4 or LiFe 0.5 Ni 0.5 P.O. 4 can be used as the barrier layer 116.
[0255] As the initial state of the model used for the calculation, LiCoO 2 and LiFePO 4 7B shows the structure of LiCoO 2 and LiFe 0.5 MPO 4 (M=Mn or Ni, specifically LiFe 0.5 Mn 0.5 P.O. 4 or LiFe 0.5 Ni 0.5 P.O. 4 ), and the bonded structure.
[0256] In these structure models, the potential difference before and after the extraction of Li (corresponding to the potential difference during charging) was calculated. 2 , LiFePO 4 (sometimes referred to as LFP), LiCoO 2 and LiFePO 4 and a stacked structure, LiCoO 2 and LiFePO 4 1 shows a graph of theoretical capacity vs. charging voltage for a structure in which LiCoO 2 and LiFePO 4 and a stacked structure, LiCoO 2 and LiFePO 4 The mixed structure is LiCoO 2 and LiFePO 4 In Figure 8B, LiCoO 2 , LiFe 0.5 Mn 0.5 P.O. 4 (sometimes referred to as LFMP), LiCoO 2 1 shows a graph of theoretical capacity vs. charging voltage for a structure in which LiCoO and LFMP are stacked. 2 The laminated structure of LiCoO 2 and LFMP are included in the bonded structure. 2 , LiFe 0.5 Ni 0.5 P.O. 4 (sometimes referred to as LFNP), LiCoO 2 1 shows a graph of theoretical capacity vs. charging voltage for a structure in which LiCoO and LFNP are stacked. 2 The structure in which LFNP is laminated with LiCoO 2 and LFNP are included in the bound structure.
[0257] As shown in Figures 8(A), (B), and (C), LiFePO 4 LiFePO 4 When part of the Fe in LiFePO is replaced with Mn, the charging voltage is higher. 4 It was confirmed that when a part of the Fe in the above-mentioned battery was replaced with Ni, the charging voltage tended to be even higher.
[0258] This embodiment mode can be implemented in appropriate combination with other embodiment modes.
[0259] Embodiment 4 In this embodiment, an example of a manufacturing method of a first material that functions as a positive electrode active material of one embodiment of the present invention will be described with reference to FIGS. 9 to 11. In addition, the positive electrode active material of one embodiment of the present invention will be described with reference to FIGS.
[0260] [Method 1 for Producing Positive Electrode Active Material] <Step S11> In step S11 shown in FIG. 9A, a lithium source (Li source) and a transition metal source (M source) are prepared as starting materials for lithium and transition metal, respectively.
[0261] As the lithium source, it is preferable to use a compound containing lithium, such as lithium carbonate, lithium hydroxide, lithium nitrate, or lithium fluoride. It is preferable that the lithium source has high purity, and for example, it is recommended to use a material with a purity of 99.99% or higher.
[0262] The transition metal can be selected from elements in Groups 4 to 13 of the periodic table, and for example, at least one of manganese, cobalt, and nickel is used. The transition metal may be only cobalt, only nickel, two elements (cobalt and manganese), two elements (cobalt and nickel), or three elements (cobalt, manganese, and nickel). When only cobalt is used, the resulting positive electrode active material has lithium cobalt oxide (LCO), and when three elements (cobalt, manganese, and nickel) are used, the resulting positive electrode active material has lithium nickel-cobalt-manganese oxide (NCM).
[0263] As the transition metal source, it is preferable to use a compound containing the above transition metal, and for example, an oxide or hydroxide of the metal exemplified above as the transition metal can be used. As a cobalt source, cobalt oxide, cobalt hydroxide, etc. can be used. As a manganese source, manganese oxide, manganese hydroxide, etc. can be used. As a nickel source, nickel oxide, nickel hydroxide, etc. can be used. As an aluminum source, aluminum oxide, aluminum hydroxide, etc. can be used.
[0264] The transition metal source preferably has a high purity, for example, a material with a purity of 3N (99.9%) or higher, preferably 4N (99.99%) or higher, more preferably 4N (99.995%) or higher, and even more preferably 5N (99.999%) or higher. By using a high-purity material, impurities in the positive electrode active material can be controlled. As a result, the capacity and / or reliability of the secondary battery can be increased.
[0265] In addition, it is preferable that the transition metal source has high crystallinity, for example, single crystal grains. The crystallinity of the transition metal source can be evaluated using TEM (transmission electron microscope) images, STEM (scanning transmission electron microscope) images, HAADF-STEM (high-angle annular dark-field scanning transmission electron microscope) images, ABF-STEM (annular bright-field scanning transmission electron microscope) images, etc., or by X-ray diffraction (XRD), electron diffraction, neutron diffraction, etc. Note that the above-mentioned methods for evaluating crystallinity can be applied not only to transition metal sources but also to evaluating the crystallinity of other sources.
[0266] When two or more transition metal sources are used, it is preferable to prepare them in a mixing ratio that allows the two or more transition metal sources to have a layered rock salt type crystal structure.
[0267] <Step S12> Next, in step S12 shown in FIG. 9A , the lithium source and the transition metal source are crushed and mixed to prepare a mixed material. Crushing and mixing can be performed by either a dry or wet method. The wet method is preferred because it allows for smaller crushing. When using the wet method, a solvent is prepared. Examples of solvents that can be used include ketones such as acetone, alcohols such as ethanol and isopropanol, ether, dioxane, acetonitrile, and N-methyl-2-pyrrolidone (NMP). It is more preferable to use an aprotic solvent that is less likely to react with lithium. In this embodiment, dehydrated acetone with a purity of 99.5% or higher is used. It is preferable to mix the lithium source and the transition metal source in dehydrated acetone with a purity of 99.5% or higher, with a water content reduced to 10 ppm or less, and then crush and mix the mixture. Using dehydrated acetone with the above purity can reduce potential impurities.
[0268] A ball mill, a bead mill, or the like can be used as a means for mixing, etc. When using a ball mill, it is preferable to use alumina balls or zirconia balls as grinding media. Zirconia balls are preferable because they emit less impurities. Furthermore, when using a ball mill, a bead mill, or the like, it is preferable to set the peripheral speed to 100 mm / s or more and 2000 mm / s or less in order to suppress contamination from the media. In this embodiment, the peripheral speed is set to 838 mm / s (rotation speed 400 rpm, ball mill diameter 40 mm).
[0269] <Step S13> Next, in step S13 shown in FIG. 9A , the mixed material is heated. The heating temperature is preferably 800°C or higher and 1100°C or lower, more preferably 900°C or higher and 1000°C or lower, and even more preferably about 950°C. If the temperature is too low, the decomposition and melting of the lithium source and the transition metal source may be insufficient. On the other hand, if the temperature is too high, defects may occur due to lithium evaporation from the lithium source and / or excessive reduction of the metal used as the transition metal source. For example, when cobalt is used as the transition metal, excessive reduction can cause cobalt to change from trivalent to divalent, which can induce oxygen defects.
[0270] The heating time is preferably from 1 hour to 100 hours, more preferably from 2 hours to 20 hours.
[0271] The temperature rise rate depends on the heating temperature reached, but is preferably 80° C. / h to 250° C. / h. For example, when heating at 1000° C. for 10 hours, the temperature rise rate should be 200° C. / h.
[0272] The heating atmosphere is preferably an atmosphere with little water, such as dry air, and for example, an atmosphere with a dew point of -50°C or less, more preferably an atmosphere with a dew point of -80°C or less. In this embodiment, heating is performed in an atmosphere with a dew point of -93°C. In addition, in order to suppress impurities that may be mixed into the material, the CH 4 , CO, CO 2 , and H 2 The impurity concentrations of the above should be 5 ppb (parts per billion) or less.
[0273] An oxygen-containing atmosphere is preferred as the heating atmosphere. For example, dry air can be continuously introduced into the reaction chamber. In this case, the flow rate of the dry air is preferably 10 L / min. The method of continuously introducing oxygen into the reaction chamber and allowing oxygen to flow through the reaction chamber is called flow.
[0274] When the heating atmosphere is an atmosphere containing oxygen, a method of not allowing oxygen to flow may be used. For example, a method of reducing the pressure of the reaction chamber and then filling it with oxygen to prevent the oxygen from entering or leaving the reaction chamber may be used, which is called purging. For example, the reaction chamber may be reduced in pressure to -970 hPa and then filled with oxygen to 50 hPa.
[0275] After heating, the material may be cooled naturally, but it is preferable that the time required for the temperature to drop from the specified temperature to room temperature is within a range of 10 to 50 hours. However, cooling to room temperature is not necessarily required, as long as the material is cooled to a temperature acceptable for the next step.
[0276] The heating in this step may be carried out using a rotary kiln or a roller hearth kiln. Heating in a rotary kiln can be carried out with stirring in either a continuous or batch system.
[0277] The crucible or sheath used during heating is preferably made of a highly heat-resistant material such as alumina (aluminum oxide), mullite / cordierite, magnesia, or zirconia. An alumina crucible is preferable because it is a material that does not easily release impurities. In this embodiment, an alumina crucible with a purity of 99.9% is preferably used. It is preferable to heat the crucible or sheath with a lid. Heating with a lid can prevent the material from volatilizing.
[0278] After heating, the material may be crushed and sieved as necessary. When recovering the heated material, it may be transferred from the crucible to a mortar and then recovered. It is preferable to use an alumina mortar. Alumina mortars are made of a material that does not easily release impurities. Specifically, an alumina mortar with a purity of 90% or more, preferably 99% or more, is used. Heating conditions equivalent to those of step S13 can also be applied to heating steps other than step S13, which will be described later.
[0279] <Step S14> By the above steps, a composite oxide containing a transition metal (LiMO) is obtained in step S14 shown in FIG. 9A. 2 The composite oxide can be obtained by 2The composition is not strictly limited to Li:M:O=1:1:2, as long as it has a crystalline structure of a lithium composite oxide represented by the formula: 2 However, the composition is not strictly limited to Li:Co:O=1:1:2.
[0280] Although the example of producing the composite oxide by the solid phase method in steps S11 to S14 has been shown, the composite oxide may also be produced by a coprecipitation method or a hydrothermal method.
[0281] <Step S15> Next, in step S15 shown in Fig. 9A, the composite oxide is heated. Because this is the first heating of the composite oxide, the heating in step S15 may be referred to as initial heating. Alternatively, because this heating is performed before step S20 described below, it may be referred to as preheating or pretreatment.
[0282] The initial heating may cause lithium to be desorbed from a part of the lithium composite oxide in step 14. It is also expected to have the effect of increasing the crystallinity of the lithium composite oxide. Furthermore, since the lithium source and / or the transition metal M prepared in step S11 or the like contains impurities, the initial heating can reduce the amount of these impurities in the lithium composite oxide in step 14.
[0283] After the initial heating, the surface of the composite oxide becomes smooth. A smooth surface refers to a state in which there are few irregularities, the composite oxide is rounded overall, and the corners are also rounded. Furthermore, a state in which there is little foreign matter adhering to the surface is called smooth. Foreign matter is thought to be a cause of irregularities, so it is preferable that no foreign matter adheres to the surface. A smooth active material can have a surface roughness of at least 10 nm or less, preferably less than 3 nm, when surface irregularity information is quantified from measurement data in a cross section observed with a scanning transmission electron microscope (STEM).
[0284] The initial heating is performed after the composite oxide is completed, and the initial heating is performed to smooth the surface, which reduces deterioration after charge and discharge. For the initial heating to smooth the surface, there is no need to prepare a lithium source.
[0285] Alternatively, in the initial heating step for smoothing the surface, it is not necessary to provide a source of the additive element.
[0286] Alternatively, in the initial heating step for smoothing the surface, no flux agent needs to be prepared.
[0287] The lithium source or transition metal source prepared in step S11 or the like may contain impurities. By initial heating, it is possible to reduce the amount of impurities in the composite oxide completed in step S14.
[0288] The heating conditions for this step may be any conditions that result in a smooth surface of the composite oxide. For example, the heating conditions may be selected from those described in step S13. Regarding the heating conditions, the heating temperature for this step may be lower than the temperature for step S13 in order to maintain the crystalline structure of the composite oxide. Furthermore, the heating time for this step may be shorter than the time for step S13 in order to maintain the crystalline structure of the composite oxide. For example, heating may be performed at a temperature of 700°C or higher and 1000°C or lower for 2 hours or longer and 20 hours or shorter.
[0289] The heating in step S13 may cause a temperature difference between the surface and the interior of the composite oxide. The temperature difference may induce a contraction difference. It is also thought that the temperature difference causes a difference in fluidity between the surface and the interior, resulting in a contraction difference. The energy associated with the contraction difference causes an internal stress difference in the composite oxide. The internal stress difference is also called strain, and this energy is sometimes called strain energy. The internal stress is removed by the initial heating in step S15; in other words, the strain energy is thought to be homogenized by the initial heating in step S15. When the strain energy is homogenized, the strain in the composite oxide is alleviated. Therefore, the surface of the composite oxide may become smoother after step S15. This is also called an improved surface. In other words, it is thought that the contraction difference that occurred in the composite oxide is alleviated after step S15, resulting in a smoother surface of the composite oxide.
[0290] Furthermore, the difference in shrinkage may cause microscopic deviations in the composite oxide, such as deviations in crystals. This step is preferably carried out in order to reduce such deviations. This step makes it possible to equalize the deviations in the composite oxide. Equalizing the deviations may result in a smoother surface of the composite oxide. This is also referred to as the alignment of crystal grains. In other words, it is believed that step S15 reduces deviations in the crystals and other components of the composite oxide, resulting in a smoother surface of the composite oxide.
[0291] When a composite oxide with a smooth surface is used as a positive electrode active material, deterioration during charge and discharge in a secondary battery is reduced, and cracking of the positive electrode active material can be prevented.
[0292] The smooth surface of a composite oxide can be defined as a surface roughness of at least 10 nm or less, preferably less than 3 nm, when surface irregularity information is quantified from measurement data at a cross section of the composite oxide. The cross section is, for example, a cross section obtained when observing with a scanning transmission electron microscope (STEM).
[0293] Alternatively, a composite oxide containing lithium, a transition metal, and oxygen that has been synthesized in advance may be used in step S14. In this case, steps S11 to S13 can be omitted. By performing step S15 on a composite oxide that has been synthesized in advance, a composite oxide with a smooth surface can be obtained.
[0294] It is possible that the lithium in the composite oxide is reduced by the initial heating. Due to the reduction in lithium, it is possible that the additive element, which will be described in the next step S20, etc., becomes more easily incorporated into the composite oxide.
[0295] <Step S20> An additional element X may be added to a composite oxide having a smooth surface, as long as it can form a layered rock salt crystal structure. Adding the additional element X to a composite oxide having a smooth surface allows the additional element to be added uniformly. Therefore, it is preferable to add the additional element after initial heating. The step of adding the additional element will be described with reference to FIGS. 9B and 9C.
[0296] 9B, an additive element source (X source) to be added to the composite oxide is prepared. A lithium source may be prepared together with the additive element source.
[0297] The additive element may be one or more selected from nickel, cobalt, magnesium, calcium, chlorine, fluorine, aluminum, manganese, titanium, zirconium, yttrium, vanadium, iron, chromium, niobium, lanthanum, hafnium, zinc, silicon, sulfur, phosphorus, boron, and arsenic. The additive element may be one or more selected from bromine and beryllium. However, since bromine and beryllium are toxic to living organisms, it is preferable to use the additive elements described above.
[0298] When magnesium is selected as the additive element, the source of the additive element can be called a magnesium source. As the magnesium source, magnesium fluoride, magnesium oxide, magnesium hydroxide, magnesium carbonate, etc. can be used. Furthermore, a plurality of the above-mentioned magnesium sources may be used.
[0299] When fluorine is selected as the additive element, the source of the additive element can be called a fluorine source. Examples of the fluorine source include lithium fluoride (LiF) and magnesium fluoride (MgF 2 ), aluminum fluoride (AlF 3 ), titanium fluoride (TiF 4 ), cobalt fluoride (CoF 2 , CoF 3 ), nickel fluoride (NiF 2 ), zirconium fluoride (ZrF 4 ), vanadium fluoride (VF 5 ), manganese fluoride, iron fluoride, chromium fluoride, niobium fluoride, zinc fluoride (ZnF 2 ), calcium fluoride (CaF 2 ), sodium fluoride (NaF), potassium fluoride (KF), barium fluoride (BaF 2 ), cerium fluoride (CeF 2 ), lanthanum fluoride (LaF 3 ), or sodium aluminum hexafluoride (Na 3 AlF 6 Among these, lithium fluoride is preferred because it has a relatively low melting point of 848° C. and is easily melted in the heating step described below.
[0300] Magnesium fluoride can be used as both a fluorine source and a magnesium source, and lithium fluoride can be used as a lithium source. Another lithium source that can be used in step S21 is lithium carbonate.
[0301] The fluorine source may also be gaseous, such as fluorine (F 2 ), fluorocarbon, sulfur fluoride, or oxygen fluoride (OF 2 , O 2 F 2 , O 3 F 2 , O 4 F 2 , O 2 F) or the like may be used and mixed into the atmosphere in the heating step described below. Also, a plurality of the above-mentioned fluorine sources may be used.
[0302] In this embodiment, lithium fluoride (LiF) is prepared as the fluorine source, and magnesium fluoride (MgF) is prepared as the fluorine source and magnesium source. 2 Lithium fluoride and magnesium fluoride are prepared as LiF:MgF 2 Mixing them at a molar ratio of about LiF:MgF = 65:35 has the greatest effect of lowering the melting point (see Non-Patent Document 4). On the other hand, if the amount of lithium fluoride is too high, there is a concern that the lithium will be in excess and the cycle characteristics will deteriorate. Therefore, the molar ratio of lithium fluoride and magnesium fluoride is set to LiF:MgF 2 =x:1 (0≦x≦1.9), and LiF:MgF 2 =x:1 (0.1≦x≦0.5) is more preferable, and LiF:MgF 2 = x: 1 (x = near 0.33) is more preferable. Note that "near" refers to a value that is greater than 0.9 times and less than 1.1 times the value.
[0303] 9B, the magnesium source and the fluorine source are pulverized and mixed. This step can be performed under pulverization and mixing conditions selected from those described in step S12.
[0304] If necessary, a heating step may be performed after step S22. The heating step can be performed under heating conditions selected from those described in step S13. The heating time is preferably 2 hours or more, and the heating temperature is preferably 800°C or higher and 1100°C or lower.
[0305] 9B, the pulverized and mixed materials are collected to obtain an additive element source (X source). The additive element source shown in step S23 includes a plurality of starting materials and can be called a mixture.
[0306] The particle size of the mixture is preferably D50 (median diameter) of 600 nm to 20 μm, more preferably 1 μm to 10 μm. Even when a single material is used as the additive element source, the D50 (median diameter) is preferably 600 nm to 20 μm, more preferably 1 μm to 10 μm.
[0307] Such a finely powdered mixture (including the case where only one type of additive element is contained) makes it easier to uniformly adhere the mixture to the surface of the composite oxide particles when mixed with the composite oxide in a later step. Uniform adhesion of the mixture to the surface of the composite oxide is preferable because it makes it easier to uniformly distribute or diffuse the additive element in the surface layer portion of the composite oxide after heating. The region where the additive element is distributed can also be referred to as the surface layer portion. If there is a region in the surface layer that does not contain the additive element, it may be difficult to obtain the O3'-type crystal structure described below in the charged state. Although fluorine has been used in the explanation, fluorine may also be chlorine, and the term "halogen" can be used to refer to both.
[0308] <Step S21> A step different from that shown in Fig. 9B will be described with reference to Fig. 9C. In step S21 shown in Fig. 9C, four types of additive element sources to be added to the composite oxide are prepared. That is, the types of additive element sources in Fig. 9C are different from those in Fig. 9B. A lithium source may be prepared together with the additive element sources.
[0309] As sources of four additive elements, a magnesium source (Mg source), a fluorine source (F source), a nickel source (Ni source), and an aluminum source (Al source) are prepared. The magnesium source and the fluorine source can be selected from the compounds described with reference to FIG. 9B . Nickel oxide, nickel hydroxide, etc. can be used as the nickel source. Aluminum oxide, aluminum hydroxide, etc. can be used as the aluminum source.
[0310] <Step S22> and <Step S23> Next, step S22 and step S23 shown in FIG. 9C are the same as the steps described with reference to FIG. 9B.
[0311] 9A , the composite oxide and an additive element source (X source) are mixed. The ratio of the number of transition metal atoms M in the composite oxide containing lithium, transition metal, and oxygen to the number of magnesium atoms Mg in the additive element X is preferably M:Mg=100:y (0.1≦y≦6), and more preferably M:Mg=100:y (0.3≦y≦3).
[0312] The mixing conditions in step S31 are preferably milder than those in step S12 so as not to destroy the composite oxide. For example, it is preferable to use conditions with a lower rotation speed or a shorter time than those in step S12. It can also be said that dry mixing provides milder conditions than wet mixing. For example, a ball mill, a bead mill, or the like can be used for mixing. When using a ball mill, it is preferable to use zirconia balls as the media.
[0313] In this embodiment, dry mixing is performed in a ball mill using zirconia balls with a diameter of 1 mm at 150 rpm for 1 hour in a dry room with a dew point of −100° C. or higher and −10° C. or lower.
[0314] <Step S32> Next, in step S32 of Fig. 9A, the mixed materials are collected to obtain a mixture 903. When collecting the materials, they may be crushed and then sieved, if necessary.
[0315] In this embodiment, a method is described in which lithium fluoride as a fluorine source and magnesium fluoride as a magnesium source are added to a composite oxide that has undergone initial heating. However, the present invention is not limited to the above method. In step S11, that is, in the stage of the starting materials for the composite oxide, a magnesium source and a fluorine source can be added to the lithium source and the transition metal source. Thereafter, in step S13, heating is performed to obtain LiMO with added magnesium and fluorine. 2 In this case, it is not necessary to separate the steps S11 to S14 from the steps S21 to S23. This method is simple and has high productivity.
[0316] Alternatively, lithium cobalt oxide to which magnesium and fluorine have been added in advance may be used. If lithium cobalt oxide to which magnesium and fluorine have been added is used, steps S11 to S32 and step S20 can be omitted. This method can be said to be simple and highly productive.
[0317] Alternatively, a magnesium source and a fluorine source may be further added to lithium cobalt oxide to which magnesium and fluorine have been added in advance according to step S20 of FIG. 9B, or a magnesium source, a fluorine source, a nickel source, and an aluminum source may be further added according to step S20 of FIG. 9C.
[0318] 9A, the mixture 903 is heated. The heating conditions can be selected from those described in step S13. The heating time is preferably 2 hours or more.
[0319] Here, a supplementary note about the heating temperature will be given. The lower limit of the heating temperature in step S33 is 2 The temperature at which the reaction between the LiMO and the additive element source proceeds must be equal to or higher than the temperature at which the reaction between the LiMO and the additive element source proceeds. 2 The temperature may be lower than the melting point of these materials as long as it is a temperature at which interdiffusion between the elements contained in the oxide and the elements contained in the additive element source occurs. m 0.757 times (Tammann temperature T d ) solid-phase diffusion occurs. Therefore, the heating temperature in step S33 should be 500° C. or higher.
[0320] Of course, the reaction is more likely to proceed when the temperature is equal to or higher than the temperature at which at least a part of the mixture 903 melts. For example, LiF and MgF 2 When LiF and MgF 2 The eutectic point of the alloy is around 742° C. Therefore, it is preferable that the lower limit of the heating temperature in step S33 is 742° C. or higher.
[0321] Also, LiCoO 2 :LiF:MgF 2 A mixture 903 obtained by mixing the components so that the molar ratio was 100:0.33:1 exhibits an endothermic peak at around 830° C. in differential scanning calorimetry (DSC). Therefore, the lower limit of the heating temperature is more preferably 830° C. or higher.
[0322] A higher heating temperature is preferable because the reaction proceeds more easily, the heating time is shorter, and productivity is higher.
[0323] The upper limit of heating temperature is LiMO 2 Decomposition temperature of LiCoO 2 The decomposition temperature of LiMO is less than 1130°C. At temperatures close to the decomposition temperature, a small amount of LiMO 2 Therefore, the temperature is more preferably 1000°C or lower, even more preferably 950°C or lower, and even more preferably 900°C or lower.
[0324] Taking these factors into consideration, the heating temperature in step S33 is preferably 500°C or higher and 1130°C or lower, more preferably 500°C or higher and 1000°C or lower, even more preferably 500°C or higher and 950°C or lower, and even more preferably 500°C or higher and 900°C or lower. Also, it is preferably 742°C or higher and 1130°C or lower, more preferably 742°C or higher and 1000°C or lower, even more preferably 742°C or higher and 950°C or lower, and even more preferably 742°C or higher and 900°C or lower. Also, it is preferably 800°C or higher and 1100°C or lower, or 830°C or higher and 1130°C or lower, more preferably 830°C or higher and 1000°C or lower, even more preferably 830°C or higher and 950°C or lower, and even more preferably 830°C or higher and 900°C or lower. The heating temperature in step S33 is preferably higher than that in step S13.
[0325] Furthermore, when the mixture 903 is heated, it is preferable to control the partial pressure of fluorine or fluoride resulting from the fluorine source or the like within an appropriate range.
[0326] In the manufacturing method described in this embodiment, some materials, for example, LiF, which is a fluorine source, may function as a flux. This function allows the heating temperature to be controlled to the temperature of the composite oxide (LiMO). 2 ) can be heated to a temperature lower than the decomposition temperature, for example, 742°C to 950°C, and additive elements such as magnesium can be distributed in the surface layer, thereby producing a positive electrode active material with good characteristics.
[0327] However, since LiF has a lower specific gravity in a gaseous state than oxygen, there is a possibility that LiF will volatilize when heated, and if it volatilizes, the amount of LiF in the mixture 903 will decrease. This will weaken its function as a flux. Therefore, it is necessary to heat while suppressing the volatilization of LiF. Even if LiF is not used as a fluorine source, etc., LiMO 2 There is a possibility that Li on the surface reacts with F in the fluorine source to produce LiF, which may then volatilize. Therefore, even if a fluoride with a higher melting point than LiF is used, it is still necessary to suppress volatilization.
[0328] Therefore, it is preferable to heat the mixture 903 in an atmosphere containing LiF, that is, to heat the mixture 903 in a state where the partial pressure of LiF is high in the heating furnace. By heating in this manner, it is possible to suppress the volatilization of LiF in the mixture 903.
[0329] The heating in this step is preferably performed so as not to stick together the mixture 903. If the mixture 903 sticks together during heating, the contact area with oxygen in the atmosphere decreases, and the route along which the added element (for example, fluorine) diffuses is blocked, which may result in poor distribution of the added element (for example, magnesium and fluorine) in the surface layer portion.
[0330] Furthermore, it is believed that uniform distribution of the additive element (e.g., fluorine) in the surface layer portion results in a smooth cathode active material with minimal irregularities. Therefore, in order to maintain the smooth surface after heating in step S15 in this process or to make it even smoother, it is better for the particles not to adhere to each other.
[0331] Furthermore, when heating in a rotary kiln, it is preferable to control the flow rate of the oxygen-containing atmosphere in the kiln during heating. For example, it is preferable to reduce the flow rate of the oxygen-containing atmosphere, or to first purge the atmosphere and then not flow the atmosphere after introducing the oxygen atmosphere into the kiln. Flowing oxygen may cause the fluorine source to evaporate, which is undesirable in terms of maintaining surface smoothness.
[0332] When heating is performed using a roller hearth kiln, the mixture 903 can be heated in an atmosphere containing LiF by placing a lid on a container containing the mixture 903, for example.
[0333] The heating time is determined by the heating temperature, the LiMO 2 It varies depending on the size and composition of LiMO. 2 If the size of is small, LiMO 2 A lower temperature or shorter time may be more preferable than when the magnitude of
[0334] The composite oxide (LiMO) in step S14 of FIG. 2 When the median diameter (D50) of the powder is about 12 μm, the heating temperature is preferably, for example, 600° C. or higher and 950° C. or lower. The heating time is preferably, for example, 3 hours or higher, more preferably 10 hours or higher, and even more preferably 60 hours or higher. The cooling time after heating is preferably, for example, 10 hours or higher and 50 hours or lower.
[0335] On the other hand, the composite oxide (LiMO) 2 When the median diameter (D50) of the sintered body is about 5 μm, the heating temperature is preferably, for example, 600° C. or higher and 950° C. or lower. The heating time is preferably, for example, 1 hour or higher and 10 hours or lower, and more preferably about 2 hours. The cooling time after heating is preferably, for example, 10 hours or higher and 50 hours or lower.
[0336] 9A, the heated material is recovered and crushed as necessary to obtain positive electrode active material 115. At this time, it is preferable to further sieve recovered positive electrode active material 115.
[0337] Through the above steps, the positive electrode active material 115 of one embodiment of the present invention can be manufactured. The positive electrode active material of one embodiment of the present invention has a smooth surface.
[0338] [Method 2 for Producing Positive Electrode Active Material] Next, a method for carrying out the present invention, which is different from Method 1 for Producing Positive Electrode Active Material, will be described.
[0339] In FIG. 10, steps S11 to S15 are performed in the same manner as in FIG. 9A to obtain a composite oxide (LiMO) with a smooth surface. 2 ) to prepare.
[0340] <Step S20a> As described above, the additive element X may be added to the composite oxide to the extent that a layered rock salt type crystal structure can be formed. In this production method 2, however, a step of adding the additive element in two or more batches will be described with reference to FIG. 11A as well.
[0341] <Step S21> Fig. 11A shows the details of step S20a. In step S21, a first additive element source (X1 source) is prepared. The X1 source can be selected from the additive elements X described in step S21 shown in Fig. 9B. For example, one or more elements selected from magnesium, fluorine, and calcium can be used as the additive element X1. Fig. 11A illustrates the case where a magnesium source (Mg source) and a fluorine source (F source) are used as the additive element source (X1 source).
[0342] Steps S21 to S23 shown in Fig. 11A can be fabricated under the same conditions as steps S21 to S23 shown in Fig. 9B. As a result, an additional element source (X1 source) can be obtained in step S23. The additional element source (X1 source) is used as the X1 source in step S20a shown in Fig. 10.
[0343] Steps S31 to S33 shown in FIG. 10 can be fabricated in the same manner as steps S31 to S33 shown in FIG. 9A.
[0344] <Step S34a> Next, the material heated in step S33 shown in Fig. 10 is recovered to prepare a composite oxide containing the additional element X1. This is also called a second composite oxide to distinguish it from the composite oxide in step S14.
[0345] <Step S40> A second additive element source (X2 source) is added in step S40 shown in Fig. 10. Details of step S40 will be described with reference to Figs. 11B and 11C.
[0346] <Step S41> In step S41 shown in FIG. 11B, a second additive element source (X2 source) is prepared. The X2 source can be selected from the additive elements X described in step S21 shown in FIG. 9B. For example, one or more elements selected from nickel, titanium, boron, zirconium, and aluminum can be suitably used as the additive element X2. FIG. 11B illustrates an example in which a nickel source and an aluminum source are used as the additive element source (X2 source).
[0347] Steps S41 to S43 shown in Fig. 11B can be fabricated under the same conditions as steps S21 to S23 shown in Fig. 9B. As a result, an additional element source (X2 source) can be obtained in step S43.
[0348] 11C shows a modified example of the steps described with reference to FIG. 11B. In step S41 shown in FIG. 11C, a nickel source (Ni source) and an aluminum source (Al source) are prepared, and in step S42a, they are independently pulverized. As a result, in step S43, a plurality of second additive element sources (X2 sources) are prepared. The steps of FIG. 11C differ from those of FIG. 11B in that the additive elements are independently pulverized in step S42a.
[0349] <Steps S51 to S53> Next, steps S51 to S53 shown in Fig. 10 can be performed under the same conditions as steps S31 to S34 shown in Fig. 9A. The conditions for step S53, which is a heating step, may be a lower temperature and a shorter time than those for step S33. Through the above steps, step S53 can produce the positive electrode active material 115 of one embodiment of the present invention. The positive electrode active material of one embodiment of the present invention has a smooth surface.
[0350] 10 and 11 , in the preparation method 2, the additive element to the composite oxide is introduced separately as a first additive element X1 and a second additive element X2. By introducing the additive elements separately, the depth profile of each additive element can be changed. For example, it is possible to profile the first additive element so that its concentration is higher in the surface layer portion than in the interior, and profile the second additive element so that its concentration is higher in the interior than in the surface layer portion.
[0351] After the initial heating described in this embodiment, a positive electrode active material with a smooth surface can be obtained.
[0352] The initial heating shown in this embodiment is performed on the composite oxide. Therefore, the initial heating is preferably performed at a temperature lower than the heating temperature for obtaining the composite oxide and for a time shorter than the heating time for obtaining the composite oxide. When an additional element is added to the composite oxide, it is preferable to perform the addition step after the initial heating. The addition step can be divided into two or more steps. Following this step order is preferable because the surface smoothness obtained by the initial heating is maintained. When the composite oxide contains cobalt as a transition metal, it can be interpreted as a composite oxide containing cobalt.
[0353] [Structure of Positive Electrode Active Material] Positive electrode active materials of embodiments of the present invention will be described with reference to FIGS.
[0354] 12A is a schematic top view of a positive electrode active material 115 according to one embodiment of the present invention. FIG. 12B is a schematic cross-sectional view taken along line A-B in FIG.
[0355] <Contained Elements and Distribution> The positive electrode active material 115 contains lithium, a transition metal, oxygen, and an additive element. The additive element may be an element different from the transition metal contained in the positive electrode active material 115. That is, the positive electrode active material 115 contains LiMO. 2 It can be said that the compound oxide represented by the formula (I) is added with elements other than M.
[0356] The transition metal contained in the positive electrode active material 115 is preferably a metal capable of forming a layered rock-salt composite oxide belonging to the space group R-3m with lithium, such as manganese, cobalt, or at least one of nickel. That is, the transition metal contained in the positive electrode active material 115 may be cobalt alone, nickel alone, a combination of cobalt and manganese, or a combination of cobalt and nickel, or three of cobalt, manganese, and nickel. That is, the positive electrode active material 115 may contain a composite oxide containing lithium and a transition metal, such as lithium cobalt oxide, lithium nickel oxide, lithium cobalt oxide in which some of the cobalt is substituted with manganese, lithium cobalt oxide in which some of the cobalt is substituted with nickel, or nickel-manganese-lithium cobalt oxide. Including nickel in addition to cobalt as a transition metal is preferable because the crystal structure becomes more stable in a charged state at a high voltage.
[0357] The additive element X contained in the positive electrode active material 115 is preferably one or more selected from nickel, cobalt, magnesium, calcium, chlorine, fluorine, aluminum, manganese, titanium, zirconium, yttrium, vanadium, iron, chromium, niobium, lanthanum, hafnium, zinc, silicon, sulfur, phosphorus, boron, and arsenic. These additive elements may further stabilize the crystalline structure of the positive electrode active material 115. That is, the positive electrode active material 115 may contain lithium cobalt oxide containing magnesium and fluorine, lithium cobalt oxide containing magnesium, fluorine, and titanium, lithium nickel-cobalt oxide containing magnesium and fluorine, lithium cobalt-aluminate containing magnesium and fluorine, nickel-cobalt-aluminate, lithium nickel-cobalt-aluminate, lithium nickel-cobalt-aluminate containing magnesium and fluorine, or lithium nickel-manganese-cobalt oxide containing magnesium and fluorine. In this specification, the additive element X may be referred to as a mixture, a part of a raw material, or the like.
[0358] As shown in FIG. 12B , the positive electrode active material 115 has a surface layer 115s and an interior 115c. The transition metal (e.g., cobalt), which is the main component of the positive electrode active material 115, is present in the surface layer 115s and the interior 115c. The additive element (e.g., magnesium) only needs to be present in at least the surface layer 115s, and may also be present in the interior 115c. The concentration of the additive element is preferably higher in the surface layer 115s than in the interior 115c. As shown by the gradation in FIG. 12B , the additive element preferably has a concentration gradient that increases from the interior to the surface. In this specification, the surface layer 115s refers to the region from the surface of the positive electrode active material 115 down to 50 nm, preferably up to 30 nm, and more preferably up to 10 nm. Surfaces created by cracks and / or fissures may also be referred to as the surface, and the region from the surface down to 50 nm, preferably up to 30 nm, and more preferably up to 10 nm is referred to as the surface layer 115s. The region deeper than the surface layer portion 115s of the positive electrode active material 115 is referred to as an interior portion 115c.
[0359] In the positive electrode active material 115 of one embodiment of the present invention, even if lithium is released from the positive electrode active material 115 due to charging, the surface layer portion 115s having a high concentration of the added element, i.e., the outer periphery of the positive electrode active material 115, is reinforced so that the layered structure formed of octahedra of cobalt and oxygen is not destroyed.
[0360] The additive element is preferably present throughout the entire surface layer 115s of the positive electrode active material 115, and more preferably present uniformly. This is because even if a portion of the surface layer 115s is reinforced, if there is a portion without reinforcement, stress may be concentrated in the unreinforced portion. If stress is concentrated in a portion of the positive electrode active material 115, defects such as cracks may occur there, which may lead to breakage of the positive electrode active material 115 and a decrease in discharge capacity.
[0361] Magnesium is divalent and is more stable at the lithium site than at the transition metal site in the layered rock-salt crystal structure, and therefore more likely to enter the lithium site. The presence of magnesium at an appropriate concentration at the lithium site in the surface layer portion 115s facilitates the maintenance of the layered rock-salt crystal structure. Furthermore, magnesium has a strong bond with oxygen, which can suppress the desorption of oxygen around the magnesium. Magnesium is preferable because, at an appropriate concentration, it does not adversely affect the insertion and desorption of lithium during charge and discharge.
[0362] However, excessive magnesium may adversely affect the insertion and desorption of lithium. Therefore, the ratio of the number of atoms of magnesium to the transition metal cobalt (Mg / Co) is preferably 0.020 or more and 0.50 or less. Furthermore, the number of atoms is preferably 0.025 or more and 0.30 or less. Furthermore, the number of atoms is preferably 0.030 or more and 0.20 or less.
[0363] Aluminum is trivalent and can exist at the transition metal site in the layered rock salt crystal structure. Aluminum can suppress the elution of surrounding cobalt. Furthermore, aluminum has a strong bond with oxygen, so it can suppress the desorption of oxygen from around the aluminum. Therefore, using aluminum as an additive element can result in a positive electrode active material 115 whose crystal structure is resistant to collapse even after repeated charge and discharge.
[0364] Fluorine is a monovalent anion, and when part of the oxygen in the surface layer portion 115s is substituted with fluorine, the lithium desorption energy is reduced. This is because the change in valence of cobalt ions accompanying lithium desorption is different, from trivalent to tetravalent in the absence of fluorine, and from divalent to trivalent in the presence of fluorine, and the oxidation-reduction potential is also different. Therefore, when part of the oxygen in the surface layer portion 115s of the positive electrode active material 115 is substituted with fluorine, it can be said that desorption and insertion of lithium ions near the fluorine is more likely to occur smoothly. Therefore, when used in a secondary battery, charge / discharge characteristics, rate characteristics, etc. are improved, which is preferable.
[0365] Titanium oxide is known to have superhydrophilicity. Therefore, by providing the cathode active material 115 with titanium oxide in the surface layer portion 115s, it is possible that the cathode active material 115 has good wettability with a highly polar solvent. When used in a secondary battery, this improves the contact at the interface between the cathode active material 115 and the highly polar electrolyte, which may suppress an increase in resistance. In this specification and the like, the electrolyte corresponds to a liquid electrolyte.
[0366] Generally, the voltage of the positive electrode increases as the charging voltage of a secondary battery increases. The positive electrode active material of one embodiment of the present invention has a stable crystal structure even at high voltages. The stable crystal structure of the positive electrode active material in a charged state can suppress a decrease in capacity due to repeated charge and discharge.
[0367] Furthermore, a short circuit in a secondary battery not only causes problems in the charging and / or discharging operations of the secondary battery, but may also lead to heat generation and fire. To achieve a safe secondary battery, it is preferable that a short circuit current be suppressed even at a high charging voltage. The positive electrode active material 115 of one embodiment of the present invention suppresses a short circuit current even at a high charging voltage. Therefore, a secondary battery that achieves both high capacity and safety can be obtained.
[0368] A secondary battery using the positive electrode active material 115 of one embodiment of the present invention preferably simultaneously satisfies high capacity, excellent charge / discharge cycle characteristics, and safety.
[0369] The concentration gradient of the added element can be evaluated, for example, by using energy dispersive X-ray spectroscopy (EDX). Among EDX measurements, measuring while scanning an area and evaluating the area two-dimensionally is sometimes called EDX area analysis. Extracting data of a linear area from EDX area analysis and evaluating the distribution of each atomic concentration in the positive electrode active material is sometimes called line analysis.
[0370] EDX area analysis (e.g., element mapping) can quantitatively analyze the concentration of the additive element in the surface layer 115s, the interior 115c, and the vicinity of the grain boundary of the positive electrode active material 115. The vicinity of the grain boundary includes a position corresponding to the surface layer on the surface forming the grain boundary. Furthermore, EDX ray analysis can analyze the concentration distribution of the additive element.
[0371] When EDX-ray analysis is performed on the positive electrode active material 115, the peak of the magnesium concentration in the surface layer portion 115s is preferably present at a depth of up to 3 nm from the surface of the positive electrode active material 115 toward the center, more preferably at a depth of up to 1 nm, and even more preferably at a depth of up to 0.5 nm.
[0372] Furthermore, the distribution of fluorine in the positive electrode active material 115 preferably overlaps with the distribution of magnesium. Therefore, when EDX ray analysis is performed, the peak of the fluorine concentration in the surface layer portion 115s is preferably present at a depth of up to 3 nm from the surface of the positive electrode active material 115 toward the center, more preferably at a depth of up to 1 nm, and even more preferably at a depth of up to 0.5 nm.
[0373] It is not necessary for all additive elements to have the same concentration distribution. For example, when the positive electrode active material 115 further contains aluminum as an additive element, it is preferable that the aluminum has a distribution slightly different from that of magnesium and fluorine. For example, when EDX-ray analysis is performed, it is preferable that the magnesium concentration peak is closer to the surface than the aluminum concentration peak in the surface layer portion 115s. For example, it is preferable that the aluminum concentration peak exists at a depth of 0.5 nm to 20 nm from the surface toward the center of the positive electrode active material 115, and more preferably at a depth of 1 nm to 5 nm.
[0374] Furthermore, when the positive electrode active material 115 is subjected to linear or area analysis, the ratio (X / M) of the additive element X to the transition metal near the grain boundary is preferably 0.020 or more and 0.50 or less. It is even more preferably 0.025 or more and 0.30 or less. It is even more preferably 0.030 or more and 0.20 or less. For example, when the additive element is magnesium and the transition metal is cobalt, the ratio of the number of magnesium atoms to the number of cobalt atoms (Mg / Co) is preferably 0.020 or more and 0.50 or less. It is even more preferably 0.025 or more and 0.30 or less. It is even more preferably 0.030 or more and 0.20 or less.
[0375] As described above, an excess of the additive element contained in the positive electrode active material 115 may adversely affect the insertion and desorption of lithium. Furthermore, this may result in an increase in resistance and a decrease in capacity when used in a secondary battery. On the other hand, if the additive element is insufficient, it may not be distributed throughout the entire surface layer portion 115s, and the effect of maintaining the crystal structure may be insufficient. Therefore, the additive element is adjusted to an appropriate concentration in the positive electrode active material 115.
[0376] For example, the positive electrode active material 115 may have a region where an excess of the additive element is unevenly distributed. The unevenly distributed region may be located inside or on the surface. The presence of such a region allows the excess additive element to be located in the unevenly distributed region, and an appropriate additive element concentration can be achieved in most of the inside and surface layers of the positive electrode active material 115. By achieving an appropriate additive element concentration in most of the inside and surface layers of the positive electrode active material 115, an increase in resistance and a decrease in capacity can be suppressed when the resulting secondary battery is used. Suppressing an increase in resistance of a secondary battery is an extremely desirable characteristic, particularly during high-rate charging and discharging.
[0377] In addition, the positive electrode active material 115 having a region where the excess additive element is unevenly distributed is allowed to have a certain amount of excess additive element mixed in during the manufacturing process, which is preferable because it provides a wider margin in production.
[0378] In this specification and the like, uneven distribution refers to the difference in the concentration of a certain element between a certain region A and a certain region B. It may also be referred to as segregation, precipitation, non-uniformity, deviation, high concentration, low concentration, or the like.
[0379] <Crystal structure> Lithium cobalt oxide (LiCoO 2 Materials having a layered rock salt type crystal structure, such as LiMO, are known to have a high discharge capacity and are excellent as positive electrode active materials for secondary batteries. 2 Examples of the composite oxide include those represented by the following formula:
[0380] It is known that the strength of the Jahn-Teller effect in composite oxides varies depending on the number of electrons in the d orbital of the transition metal.
[0381] In composite oxides containing nickel, distortion may easily occur due to the Jahn-Teller effect. 2 When LiCoO is charged and discharged at a high voltage, there is a concern that the crystal structure may be destroyed due to distortion. 2 It is suggested that the influence of the Jahn-Teller effect is small in this case, and the durability of charge and discharge at high voltages may be superior, which is preferable.
[0382] The positive electrode active material will be described with reference to Fig. 13 to Fig. 16. Fig. 13 to Fig. 16 describe the case where cobalt is used as the transition metal contained in the positive electrode active material.
[0383] <Li x CoO 2 When x is 1 in the positive electrode active material 115 of one embodiment of the present invention, the positive electrode active material 115 is in a discharged state, that is, Li x CoO 2 In the case where x = 1 in the formula (I), it is preferable that the composite oxide has a layered rock-salt type crystal structure belonging to the space group R-3m. The layered rock-salt type composite oxide has a high discharge capacity, has two-dimensional diffusion paths for lithium ions, is suitable for lithium ion insertion / extraction reactions, and is excellent as a positive electrode active material for secondary batteries. Therefore, it is particularly preferable that the inner portion 115c, which occupies the majority of the volume of the positive electrode active material 115, has a layered rock-salt type crystal structure.
[0384] In Fig. 13, O3 is added to the space group R-3m in the layered rock salt crystal structure. O3 is a crystal structure in which lithium occupies an octahedral site and CoO 2This is sometimes called the O3 type crystal structure because it has three layers. 2 The layer is an octahedral structure in which cobalt is six-coordinated with oxygen, and the structure is continuous on a plane with edge sharing. 2 The layer is sometimes referred to as a layer of cobalt and oxygen octahedra.
[0385] <Li x CoO 2 State in which x is small in the positive electrode active material 115 of one embodiment of the present invention is Li x CoO 2 The crystal structure when x is small differs from that of conventional positive electrode active materials. Here, "small x" means 0.1<x≦0.24. Figure 13 shows the crystal structure when x = 0.2.
[0386] Li x CoO 2 A conventional positive electrode active material and the positive electrode active material 115 of one embodiment of the present invention are compared with each other in terms of changes in the crystal structure with changes in x in the positive electrode active material.
[0387] <Conventional Positive Electrode Active Material> The change in the crystal structure of a conventional positive electrode active material is shown in FIG. 15. The conventional positive electrode active material shown in FIG. 15 is lithium cobalt oxide (LiCoO 2 , LCO). As described in Non-Patent Documents 1 to 3, the crystal structure of the lithium cobalt oxide shown in FIG.
[0388] In Figure 15, x CoO 2 The crystal structure of lithium cobalt oxide with x = 1 is shown with R-3m O3 attached. x = 1 corresponds to the discharged state of the secondary battery. Next, the crystal structure of lithium cobalt oxide with x = 0.5 is shown with P2 / m monoclinic O1 attached. Conventional lithium cobalt oxide has a crystal structure that belongs to the monoclinic space group P2 / m when the symmetry of lithium increases at around x = 0.5. This structure has CoO in the unit cell. 2 There is one layer. Therefore, this crystal structure is sometimes called O1 type or monoclinic O1 type.
[0389] Also Lix CoO 2 The crystal structure of lithium cobalt oxide when x = 0 is shown in the figure, along with P-3m1 trigonal O1. Conventional lithium cobalt oxide has a crystal structure that belongs to the trigonal space group P-3m1 when x = 0. This structure has CoO in the unit cell. 2 There is one layer. Therefore, this crystal structure is sometimes called O1 type or trigonal O1 type. In addition, when the trigonal crystal is converted into a composite hexagonal lattice, this crystal structure is sometimes called hexagonal O1 type.
[0390] Also Li x CoO 2 The crystal structure of lithium cobalt oxide when x = 0.12 is shown with R-3m H1-3 attached. Conventional lithium cobalt oxide has a crystal structure that belongs to the space group R-3m when x = 0.12. This structure is similar to CoO, such as trigonal O1 type. 2 and LiCoO such as R-3m O 2 It can also be said that the structure of and are stacked alternately. Therefore, this crystal structure is sometimes referred to as the H1-3 type crystal structure. Note that, since actual lithium insertion and desorption can be uneven, the H1-3 type crystal structure is observed from about x = 0.25. In addition, the number of cobalt atoms per unit cell in the H1-3 type crystal structure is actually twice that of other structures. However, in Figure 15 and other parts of this specification, the c-axis of the H1-3 type crystal structure is shown as 1 / 2 of the unit cell to facilitate comparison with other crystal structures.
[0391] As an example of the H1-3 type crystal structure, as described in Non-Patent Document 2, the coordinates of cobalt and oxygen in the unit cell can be expressed as Co (0, 0, 0.42150 ± 0.00016), O1 (0, 0, 0.27671 ± 0.00045), and O2 (0, 0, 0.11535 ± 0.00045). O1 and O2 are each oxygen atoms. Which unit cell should be used to represent the crystal structure of the positive electrode active material can be determined, for example, by Rietveld analysis of the XRD pattern. In this case, it is sufficient to adopt a unit cell that results in a small GOF (goodness of fit) value.
[0392] Li x CoO 2 When charging and discharging are repeated so that x in the formula is 0.24 or less, conventional lithium cobalt oxide undergoes repeated changes in crystal structure (i.e., non-equilibrium phase changes) between the H1-3 type crystal structure and the R-3m O3 structure in the discharged state.
[0393] However, these two crystal structures are different from CoO 2 As shown by the dotted lines and arrows in FIG. 15, in the H1-3 type crystal structure, CoO 2 The layers are significantly deviated from R-3m O3. Such dynamic structural changes can adversely affect the stability of the crystal structure.
[0394] Furthermore, the difference in volume between these two crystal structures is large: per the same number of cobalt atoms, the difference in volume between the H1-3 crystal structure and the discharged R-3mO3 crystal structure is greater than 3.5%, typically 3.9% or more.
[0395] In addition, the H1-3 type crystal structure has CoO like the trigonal O1 type. 2 There is no lithium between the layers, and CoO 2 A structure with continuous layers is likely to be unstable.
[0396] Therefore, when charging and discharging is repeated so that x becomes 0.24 or less, the crystal structure of conventional lithium cobalt oxide collapses. This collapse of the crystal structure causes a deterioration in cycle characteristics. This is because the collapse of the crystal structure reduces the number of sites where lithium can exist stably and makes it difficult for lithium to be inserted and extracted.
[0397] <Positive Electrode Active Material of One Embodiment of the Present Invention> In the positive electrode active material 115 of one embodiment of the present invention shown in FIG. 13, Li x CoO 2 The change in the crystal structure between the discharge state where x is 1 and the state where x is 0.24 or less, for example, x = 0.2, is smaller than that of conventional positive electrode active materials. More specifically, the change in the crystal structure between the discharge state where x is 1 and the state where x is 0.2, i.e., x = 0.2, is smaller than that of conventional positive electrode active materials. 2The layer misalignment can be reduced. Furthermore, the change in volume per cobalt atom can be reduced. Therefore, the positive electrode active material 115 of one embodiment of the present invention is less likely to lose its crystal structure even when repeatedly charged and discharged so that x is 0.24 or less, and excellent cycle characteristics can be achieved.
[0398] The positive electrode active material 115 of one embodiment of the present invention is Li x CoO 2 When x is 0.24 or less, the positive electrode active material 115 of one embodiment of the present invention can have a more stable crystal structure than conventional positive electrode active materials. x CoO 2 When the value of x is kept at 0.24 or less, short circuits are less likely to occur and the safety of the secondary battery is further improved, which is preferable.
[0399] Li x CoO 2 The crystal structure of lithium cobalt oxide when x is approximately 1 or 0.2 is shown in Figure 13. It is a composite oxide containing lithium cobalt oxide, cobalt as a transition metal, and oxygen. In addition to the above, it preferably contains magnesium as an additive element. It is also preferably contains a halogen such as fluorine or chlorine as an additive element.
[0400] The lithium cobalt oxide of one embodiment of the present invention has the same R-3m O3 crystal structure as conventional lithium cobalt oxide when x = 1. The lithium cobalt oxide of one embodiment of the present invention has a crystal structure different from conventional lithium cobalt oxide when x is 0.24 or less, for example, about 0.2, such that conventional lithium cobalt oxide has an H1-3 type crystal structure.
[0401] When x is about 0.2, the lithium cobalt oxide of one embodiment of the present invention has a crystal structure belonging to the trigonal space group R-3m. 2 The symmetry of the layers is the same as that of O3. Therefore, this crystal structure is called an O3'-type crystal structure. In addition, in Figure 13, R-3m O3' is added to the crystal structure when x = 0.2.
[0402] In the O3'-type crystal structure, the coordinates of cobalt and oxygen in the unit cell can be expressed in the range of Co(0,0,0.5), O(0,0,x), 0.20≦x≦0.25. Furthermore, the lattice constant of the unit cell is preferably 2.797≦a≦2.837 (Å), more preferably 2.807≦a≦2.827 (Å), typically a=2.817 (Å). The c-axis is preferably 13.681≦c≦13.881 (Å), more preferably 13.751≦c≦13.811, typically c=13.781 (Å).
[0403] As shown by the dotted line in FIG. 13, the R-3m O3 in the discharged state and the O3'-type crystal structure are different from CoO 2 There is almost no layer misalignment.
[0404] The difference in volume per the same number of cobalt atoms between R-3m O3 in a discharged state and the O3'-type crystal structure is 2.5% or less, more specifically 2.2% or less, typically 1.8%, which is a small volume difference.
[0405] In this way, in the positive electrode active material 115, Li x CoO 2 When x is small, that is, when a large amount of lithium is released, the change in crystal structure is suppressed compared to conventional positive electrode active materials. Furthermore, the change in volume is also suppressed when compared per the same number of cobalt atoms. Therefore, the positive electrode active material 115 does not easily lose its crystal structure even when repeatedly charged and discharged so that x is 0.24 or less. Therefore, the positive electrode active material 115 suppresses the decrease in charge / discharge capacity during charge / discharge cycles. Furthermore, because more lithium can be stably utilized than in conventional positive electrode active materials, the positive electrode active material 115 has a large discharge capacity per weight and per volume. Therefore, by using the positive electrode active material 115, a secondary battery with a high discharge capacity per weight and per volume can be manufactured.
[0406] The positive electrode active material 115 is Li x CoO 2 It has been confirmed that when x is 0.15 or more and 0.24 or less, the O3' type crystal structure may be present, and it is presumed that the O3' type crystal structure is present even when x is more than 0.24 and 0.27 or less. However, the crystal structure is x CoO2 Since the influence is due to factors such as the number of charge / discharge cycles, charge / discharge current, temperature, electrolyte, etc., as well as the value of x in the formula (I), the O3'-type crystal structure may be obtained regardless of the above range of x.
[0407] The positive electrode active material 115 is Li x CoO 2 When x is greater than 0.1 and equal to or less than 0.24, the entire interior of the positive electrode active material 115 does not have to have an O3′-type crystal structure, but may contain other crystal structures, or may be partially amorphous.
[0408] Also Li x CoO 2 To make the value of x small, it is generally necessary to charge at a high charging voltage. x CoO 2 In other words, a state in which x is small can be said to be a state in which the battery is charged at a high charging voltage. For example, when a conventional positive electrode active material is charged at a voltage of 4.6 V or higher relative to the potential of lithium metal in an environment of 25°C, an H1-3 crystal structure appears. Therefore, a high charging voltage relative to the potential of lithium metal can be said to be a charging voltage of 4.6 V or higher. Furthermore, in this specification and the like, unless otherwise specified, the charging voltage will be expressed relative to the potential of lithium metal.
[0409] In other words, a high charging voltage for the positive electrode active material 115 is preferable because it allows the crystal structure having the symmetry of R-3mO3 to be maintained. An example of a high charging voltage is a voltage of 4.6 V or more at 25° C. Another example of a higher charging voltage is a voltage of 4.65 V or more and 4.7 V or less at 25° C.
[0410] When the charge voltage is further increased, H1-3 type crystals may be gradually observed in the positive electrode active material 115. As described above, the crystal structure is affected by the number of charge / discharge cycles, the charge / discharge current, the electrolyte, and the like. Therefore, even when the charge voltage is lower, for example, even when the charge voltage is 4.5 V or higher and lower than 4.6 V at 25° C., the positive electrode active material 115 of one embodiment of the present invention may have an O3′ type crystal structure.
[0411] In addition, when graphite is used as the negative electrode active material in a secondary battery, the voltage of the secondary battery is lower than the above by the potential of the graphite. The potential of graphite is about 0.05 V to 0.2 V with respect to the potential of lithium metal. Therefore, in the case of a secondary battery using graphite as the negative electrode active material, the same crystal structure is maintained at a voltage obtained by subtracting the potential of graphite from the above voltage.
[0412] In addition, in O3' of FIG. 13, lithium is shown to exist at all lithium sites with equal probability, but this is not limited to this. It may exist unevenly at some lithium sites, or, for example, in the monoclinic O1 (Li 0.5 CoO 2 The distribution of lithium can be analyzed, for example, by neutron diffraction.
[0413] The O3' type crystal structure is CoO 2 Although it has random lithium between the layers, CdCl 2 It can be said that this crystal structure is similar to that of the CdCl type. 2 A similar crystal structure to the Li-type is lithium nickel oxide. 0.06 NiO 2 However, pure lithium cobaltate or layered rock salt cathode active materials containing a large amount of cobalt usually have a crystal structure similar to that of CdCl 2 It is known that it does not have a typical crystal structure.
[0414] CoO 2 The additive element, for example, magnesium, which is randomly and dilutely present between the layers, i.e., at the lithium site, turns into CoO when charged at a high voltage. 2 This has the effect of suppressing layer misalignment. 2 When magnesium is present between layers, an O3'-type crystal structure is likely to be formed. Therefore, magnesium is preferably distributed in at least the surface portion of the positive electrode active material 115 of one embodiment of the present invention, and further distributed throughout the positive electrode active material 115. In order to distribute magnesium throughout the positive electrode active material 115, heat treatment is preferably performed in the manufacturing process of the positive electrode active material 115 of one embodiment of the present invention.
[0415] However, if the heat treatment temperature is too high, cation mixing occurs, increasing the possibility that an added element, such as magnesium, will enter the cobalt site. Magnesium present in the cobalt site is ineffective in maintaining the R-3m structure during high-voltage charging. Furthermore, if the heat treatment temperature is too high, there are concerns about adverse effects such as cobalt being reduced to divalent and lithium transpiration.
[0416] Therefore, it is preferable to add a halogen compound such as a fluorine compound to lithium cobalt oxide before the heat treatment for distributing magnesium in the positive electrode active material 115. Adding the halogen compound lowers the melting point of lithium cobalt oxide. Lowering the melting point makes it easier to distribute magnesium in the positive electrode active material 115 at a temperature where cation mixing is unlikely to occur. Furthermore, the presence of a fluorine compound is expected to improve corrosion resistance against hydrofluoric acid produced by decomposition of the electrolyte.
[0417] Note that increasing the magnesium concentration above a desired value may reduce the effect on stabilizing the crystal structure. This is thought to be because magnesium enters the cobalt site in addition to the lithium site. The number of magnesium atoms in the positive electrode active material of one embodiment of the present invention is preferably 0.001 to 0.1 times the number of atoms of the transition metal, such as cobalt, more preferably more than 0.01 to less than 0.04 times, and even more preferably about 0.02 times. The magnesium concentration shown here may be, for example, a value obtained by elemental analysis of the entire particle of the positive electrode active material 115 using ICP-MS or the like, or may be based on the value of the raw material composition in the process of producing the positive electrode active material.
[0418] Lithium cobalt oxide may contain one or more metals other than cobalt (hereinafter referred to as metal Z), such as nickel, aluminum, manganese, titanium, vanadium, and chromium. Adding one or more of nickel and aluminum is particularly preferred. Manganese, titanium, vanadium, and chromium may be stable and easily tetravalent, which may contribute significantly to structural stability. Adding metal Z may make the crystal structure more stable in a charged state at a high voltage. In the positive electrode active material of one embodiment of the present invention, metal Z is preferably added at a concentration that does not significantly change the crystallinity of lithium cobalt oxide. For example, the amount is preferably such that the aforementioned Jahn-Teller effect or the like is not exhibited.
[0419] The transition metals, including nickel and manganese, and aluminum are preferably present at the cobalt site, but may be partially present at the lithium site. Magnesium is preferably present at the lithium site. Oxygen may be partially substituted with fluorine.
[0420] As the magnesium concentration of the positive electrode active material of one embodiment of the present invention increases, the capacity of the positive electrode active material may decrease. One possible cause of this is the incorporation of magnesium into lithium sites, which reduces the amount of lithium contributing to charge and discharge. Excess magnesium may also produce magnesium compounds that do not contribute to charge and discharge. By including nickel as the metal Z in addition to magnesium in the positive electrode active material of one embodiment of the present invention, the capacity per weight and per volume may be increased. Furthermore, by including aluminum as the metal Z in addition to magnesium in the positive electrode active material of one embodiment of the present invention, the capacity per weight and per volume may be increased. Furthermore, by including nickel and aluminum in addition to magnesium in the positive electrode active material of one embodiment of the present invention, the capacity per weight and per volume may be increased.
[0421] The concentrations of elements such as magnesium and metal Z contained in the positive electrode active material of one embodiment of the present invention will be discussed below.
[0422] When the positive electrode active material of one embodiment of the present invention contains magnesium in addition to element X, the stability in a high-voltage charged state is extremely high. When element X is phosphorus, the number of phosphorus atoms is preferably 1% to 20% of the number of cobalt atoms, more preferably 2% to 10%, and even more preferably 3% to 8%. In addition, the number of magnesium atoms is preferably 0.1% to 10%, more preferably 0.5% to 5%, and even more preferably 0.7% to 4% of the number of cobalt atoms. The concentrations of phosphorus and magnesium shown here may be values obtained by elemental analysis of the entire particles of the positive electrode active material using, for example, ICP-MS, or may be based on values of the composition of raw materials in the process of producing the positive electrode active material.
[0423] The number of nickel atoms in the positive electrode active material of one embodiment of the present invention is preferably 10% or less of the number of cobalt atoms, more preferably 7.5% or less, even more preferably 0.05% or more and 4% or less, and particularly preferably 0.1% or more and 2% or less. The nickel concentration shown here may be, for example, a value obtained by elemental analysis of the entire particles of the positive electrode active material using ICP-MS or the like, or may be based on the value of the composition of raw materials in the process of producing the positive electrode active material.
[0424] If the positive electrode active material 115 is charged at a high voltage for a long period of time, transition metals may leach out of the positive electrode active material 115 into the electrolyte, causing the crystal structure to collapse. However, by containing nickel in the above proportion, it may be possible to suppress the leach-out of transition metals from the positive electrode active material 115.
[0425] The number of aluminum atoms in the positive electrode active material of one embodiment of the present invention is preferably 0.05% to 4%, and more preferably 0.1% to 2%, of the number of cobalt atoms. The aluminum concentration shown here may be a value obtained by elemental analysis of the entire particles of the positive electrode active material using, for example, ICP-MS or the like, or may be based on the value of the composition of raw materials in the process of producing the positive electrode active material.
[0426] The positive electrode active material of one embodiment of the present invention preferably contains an element X, and phosphorus is preferably used as the element X. Furthermore, the positive electrode active material of one embodiment of the present invention more preferably contains a composite oxide containing phosphorus and oxygen.
[0427] When the positive electrode active material of one embodiment of the present invention includes a composite oxide containing element X, a short circuit may be less likely to occur when the positive electrode active material is maintained in a charged state at a high voltage.
[0428] When the positive electrode active material of one embodiment of the present invention contains phosphorus as the element X, hydrogen fluoride generated by decomposition of the electrolyte solution may react with the phosphorus, resulting in a decrease in the hydrogen fluoride concentration in the electrolyte solution.
[0429] The electrolyte is LiPF as a lithium salt. 6 In the case where the electrolyte contains PVDF, hydrogen fluoride may be generated by hydrolysis. Hydrogen fluoride may also be generated by the reaction of PVDF, which is used as a component of the positive electrode, with an alkali. By reducing the hydrogen fluoride concentration in the electrolyte, corrosion of the current collector and / or peeling of the coating may be suppressed. Furthermore, gelation and / or insolubilization of PVDF may be suppressed, which may result in a decrease in adhesion.
[0430] When the positive electrode active material has cracks, the presence of phosphorus, more specifically, a composite oxide containing phosphorus and oxygen, inside the cracks may inhibit the progression of the cracks.
[0431] As is clear from the oxygen atoms indicated by the arrows in Figure 13, the symmetry of the oxygen atoms is slightly different between the O3 type crystal structure and the O3' type crystal structure. Specifically, in the O3 type crystal structure, the oxygen atoms are aligned along the dotted line, whereas in the O3' type crystal structure, the oxygen atoms are not aligned strictly. This is because in the O3' type crystal structure, as lithium decreases, tetravalent cobalt increases, causing Jahn-Teller distortion to increase, resulting in CoO 6 This is because the octahedral structure of CoO is distorted. 2 This is also due to the stronger repulsion between the oxygen atoms in the layers.
[0432] <<Surface Layer Portion 115s>> Magnesium is preferably distributed throughout the particle of the positive electrode active material 115 of one embodiment of the present invention, and in addition, the magnesium concentration in the surface layer portion 115s is preferably higher than the average magnesium concentration in the entire particle. For example, the magnesium concentration in the surface layer portion 115s measured by XPS or the like is preferably higher than the average magnesium concentration in the entire particle measured by ICP-MS or the like.
[0433] Furthermore, when the positive electrode active material 115 of one embodiment of the present invention contains an element other than cobalt, for example, one or more metals selected from nickel, aluminum, manganese, iron, and chromium, the concentration of the metal near the particle surface is preferably higher than the average concentration of the entire particle. For example, the concentration of the element other than cobalt in the surface layer 115s measured by XPS or the like is preferably higher than the average concentration of the element in the entire particle measured by ICP-MS or the like.
[0434] The surface layer portion of the positive electrode active material is, so to speak, entirely composed of crystal defects. Furthermore, lithium is released from the surface during charging, making this portion prone to a lower lithium concentration than the interior. This makes the surface portion prone to instability and a breakdown of the crystal structure. A high magnesium concentration in the surface layer portion 115s can more effectively suppress changes in the crystal structure. Furthermore, a high magnesium concentration in the surface layer portion 115s can be expected to improve corrosion resistance to hydrofluoric acid produced by decomposition of the electrolyte.
[0435] The concentration of halogen such as fluorine in the surface layer portion 115s of the positive electrode active material 115 of one embodiment of the present invention is also preferably higher than the average concentration of the entire positive electrode active material 115. The presence of halogen in the surface layer portion 115s, which is a region in contact with the electrolyte, can effectively improve corrosion resistance to hydrofluoric acid.
[0436] As described above, the surface portion 115s of the positive electrode active material 115 of one embodiment of the present invention preferably has a different composition from the inner portion 115c, that is, a higher concentration of additive elements, such as magnesium and fluorine, than the inner portion 115c. Furthermore, the composition preferably has a stable crystal structure at room temperature. Therefore, the surface portion 115s may have a different crystal structure from the inner portion 115c. For example, at least a portion of the surface portion 115s of the positive electrode active material 115 of one embodiment of the present invention may have a rock-salt crystal structure. Furthermore, when the surface portion 115s and the inner portion 115c have different crystal structures, it is preferable that the crystal orientations of the surface portion 115s and the inner portion 115c roughly match.
[0437] The anions in the layered rock salt crystal and the rock salt crystal have a cubic close-packed structure (face-centered cubic lattice structure). It is estimated that the anions in the O3'-type crystal also have a cubic close-packed structure. When they contact, there is a crystal plane where the orientation of the cubic close-packed structure formed by the anions is aligned. However, the space group of the layered rock salt crystal and the O3'-type crystal is R-3m, which is different from the space group of the rock salt crystal, Fm-3m (the space group of a general rock salt crystal) and Fd-3m (the space group of a rock salt crystal with the simplest symmetry). Therefore, the Miller indices of the crystal planes that satisfy the above conditions are different between the layered rock salt crystal and the O3'-type crystal and the rock salt crystal. In this specification, when the orientation of the cubic close-packed structure formed by the anions is aligned in the layered rock salt crystal, the O3'-type crystal, and the rock salt crystal, the crystal orientation may be said to be approximately aligned.
[0438] The fact that the crystal orientations of the two regions roughly match can be determined from TEM (transmission electron microscope) images, STEM (scanning transmission electron microscope) images, HAADF-STEM (high-angle annular dark-field scanning transmission electron microscope) images, ABF-STEM (annular bright-field scanning transmission electron microscope) images, etc. X-ray diffraction (XRD), electron beam diffraction, neutron beam diffraction, etc. can also be used as materials for determination. When the crystal orientations roughly match, it can be observed in TEM images, etc. that the difference in direction between the rows of linearly alternating cations and anions is 5 degrees or less, more preferably 2.5 degrees or less. Note that light elements such as oxygen and fluorine may not be clearly observed in TEM images, etc., but in such cases, the alignment of the orientations can be determined from the arrangement of metal elements.
[0439] However, if the surface layer 115s is composed of only MgO or only a solid solution of MgO and CoO(II), it becomes difficult to insert and extract lithium. Therefore, the surface layer 115s must contain at least cobalt, and in a discharged state, it must also contain lithium, providing a path for lithium insertion and extraction. Furthermore, it is preferable that the concentration of cobalt be higher than that of magnesium.
[0440] The element X is preferably located in the surface layer portion 115s of the positive electrode active material 115 of one embodiment of the present invention. For example, the positive electrode active material 115 of one embodiment of the present invention may be covered with a coating (barrier layer) containing the element X.
[0441] <Grain Boundary> The additional element X contained in the positive electrode active material 115 of one embodiment of the present invention may be present randomly and dilutely inside the positive electrode active material 115, but it is more preferable that a part of the additional element X segregates at the grain boundary.
[0442] In other words, the concentration of the additional element X at and near the grain boundaries of the positive electrode active material 115 of one embodiment of the present invention is preferably higher than that in other regions inside the grain boundaries.
[0443] Like the particle surfaces, the grain boundaries are also planar defects. Therefore, they are prone to instability and changes in the crystal structure are likely to occur. Therefore, if the concentration of the added element X at and near the grain boundaries is high, changes in the crystal structure can be more effectively suppressed.
[0444] Furthermore, when the concentration of the additive element X is high at and near the grain boundary, even if cracks occur along the grain boundary of the positive electrode active material 115 of one embodiment of the present invention, the concentration of the additive element X becomes high near the surface where the cracks occur. Therefore, the corrosion resistance to hydrofluoric acid can be improved even in the positive electrode active material after the cracks occur.
[0445] In this specification, the vicinity of a grain boundary refers to a region within 50 nm from the grain boundary, more preferably within 35 nm from the grain boundary, even more preferably within 20 nm from the grain boundary, and most preferably within 10 nm from the grain boundary.
[0446] <Particle size> If the particle size of the positive electrode active material 115 of one embodiment of the present invention is too large, problems such as difficulty in diffusing lithium or excessive roughness of the surface of the active material layer when applied to a current collector occur. On the other hand, if the particle size is too small, problems such as difficulty in supporting the active material layer when applied to a current collector or excessive reaction with an electrolyte solution occur. Therefore, the average particle size (D50: also referred to as median diameter) is preferably 1 μm or more and 100 μm or less, more preferably 2 μm or more and 40 μm or less, and even more preferably 5 μm or more and 30 μm or less.
[0447] <Analysis Method> Whether a certain positive electrode active material is the positive electrode active material 115 of one embodiment of the present invention that exhibits an O3′-type crystal structure when charged at a high voltage can be determined by analyzing the positive electrode charged at a high voltage using XRD, electron diffraction, neutron diffraction, electron spin resonance (ESR), nuclear magnetic resonance (NMR), etc. XRD is particularly preferable in that it can analyze the symmetry of a transition metal such as cobalt contained in the positive electrode active material with high resolution, it can compare the level of crystallinity and the orientation of the crystals, it can analyze the periodic distortion of the lattice and the crystallite size, and it can obtain sufficient accuracy even when measuring a positive electrode obtained by disassembling a secondary battery as is.
[0448] As described above, the positive electrode active material 115 of one embodiment of the present invention is characterized by minimal change in crystal structure between a high-voltage charged state and a discharged state. Materials in which a crystal structure that exhibits a significant change between a high-voltage charged state and a discharged state accounts for 50 wt % or more are undesirable because they cannot withstand high-voltage charging and discharging. It should be noted that the desired crystal structure may not be achieved simply by adding an additive element. For example, even if both materials share the common feature of being lithium cobalt oxide containing magnesium and fluorine, there are cases in which the O3′-type crystal structure accounts for 60 wt % or more and cases in which the H1-3-type crystal structure accounts for 50 wt % or more when charged at a high voltage. Furthermore, at a certain voltage, the O3′-type crystal structure may be nearly 100 wt %, and further increasing the voltage may result in the H1-3-type crystal structure. Therefore, to determine whether a material is the positive electrode active material 115 of one embodiment of the present invention, analysis of the crystal structure, such as XRD, is required.
[0449] However, when a positive electrode active material is charged or discharged at a high voltage, its crystal structure may change when exposed to air. For example, it may change from an O3'-type crystal structure to an H1-3-type crystal structure. Therefore, it is preferable to handle all samples in an inert atmosphere such as an argon atmosphere.
[0450] <Charging Method> High-voltage charging for determining whether a certain composite oxide is the positive electrode active material 115 of one embodiment of the present invention can be performed, for example, by preparing a coin cell (CR2032 type, diameter 20 mm, height 3.2 mm) using a lithium counter electrode.
[0451] More specifically, the positive electrode may be prepared by coating a positive electrode current collector made of aluminum foil with a slurry containing a positive electrode active material and a conductive material.
[0452] Lithium metal can be used for the counter electrode. When a material other than lithium metal is used for the counter electrode, the potential of the secondary battery differs from the potential of the positive electrode. Unless otherwise specified, voltages and potentials in this specification refer to the potential of the positive electrode.
[0453] The electrolyte contained in the electrolytic solution was 1 mol / L lithium hexafluorophosphate (LiPF6 ) is used, and the electrolyte may be a mixture of ethylene carbonate (EC) and diethyl carbonate (DEC) in a volume ratio of EC:DEC=3:7 with 2 wt % vinylene carbonate (VC).
[0454] The separator can be made of polypropylene having a thickness of 25 μm.
[0455] The positive electrode can and the negative electrode can may be made of stainless steel (SUS).
[0456] The coin cell fabricated under the above conditions was charged at a constant current of 4.6 V and 0.5 C, followed by constant voltage charging until the current reached 0.01 C. Here, 1 C corresponds to 137 mA / g. The temperature was 25°C. After charging in this manner, the coin cell was disassembled in an argon-filled glove box and the positive electrode was removed, yielding a positive electrode active material charged at high voltage. When various analyses were subsequently performed, it was preferable to seal the cell in an argon-filled atmosphere to prevent reactions with external components. For example, XRD could be performed by sealing the cell in an airtight container in an argon atmosphere.
[0457] <XRD> Ideal powder XRD patterns calculated from the O3'-type crystal structure and H1-3-type crystal structure models using CuKα1 radiation are shown in Figures 14 and 16. For comparison, Li x CoO 2 LiCoO where x=1 2 The ideal XRD patterns calculated from the crystal structures of O3, H1-3 type, and trigonal O1 with x = 0 are also shown. 2 O3 and CoO 2 The O1 pattern was created using Reflex Powder Diffraction, a module of Materials Studio (BIOVIA), from crystal structure information obtained from the Inorganic Crystal Structure Database (ICSD) (see Non-Patent Document 5). The 2θ range was 15° to 75°, with a step size of 0.01 and a wavelength of λ1 of 1.540562 × 10. −10m and λ2 were not set, and the monochromator was single. The pattern of the H1-3 type crystal structure was similarly created from the crystal structure information described in Non-Patent Document 3. The crystal structure pattern of the O3' type crystal structure was estimated from the XRD pattern of the positive electrode active material of one embodiment of the present invention, and fitting was performed using TOPAS ver. 3 (crystal structure analysis software manufactured by Bruker), and an XRD pattern was created in the same manner as the others.
[0458] As shown in Figure 14, in the O3' type crystal structure, diffraction peaks appear at 2θ = 19.30 ± 0.20° (19.10° to 19.50°) and 2θ = 45.55 ± 0.10° (45.45° to 45.65°). More specifically, sharp diffraction peaks appear at 2θ = 19.30 ± 0.10° (19.20° to 19.40°) and 2θ = 45.55 ± 0.05° (45.50° to 45.60°). However, as shown in Figure 16, in the H1-3 type crystal structure and CoO 2 No peaks appear at these positions in O1. Therefore, the appearance of peaks at 2θ = 19.30 ± 0.20° and 2θ = 45.55 ± 0.10° in a state charged at a high voltage can be said to be a characteristic of the positive electrode active material 115 of one embodiment of the present invention.
[0459] This means that the positions at which XRD diffraction peaks appear are close between x = 1 and x ≦ 0.24. More specifically, the difference in the positions at which two or more, preferably three or more, of the main diffraction peaks of both samples is 2θ = 0.7 or less, more preferably 2θ = 0.5 or less.
[0460] Note that the positive electrode active material 115 of one embodiment of the present invention is LixCoO 2When x in the formula is small, the cathode active material 115 has an O3'-type crystal structure, but not all of the cathode active material 115 may have an O3'-type crystal structure. It may contain other crystal structures, or a portion may be amorphous. However, when Rietveld analysis is performed on the XRD pattern, the O3'-type crystal structure is preferably 50 wt% or more, more preferably 60 wt% or more, and even more preferably 66 wt% or more. If the O3'-type crystal structure is 50 wt% or more, more preferably 60 wt% or more, and even more preferably 66 wt% or more, it can be a cathode active material with sufficiently excellent cycle characteristics.
[0461] Furthermore, even after 100 or more charge / discharge cycles from the start of cycle measurement, when Rietveld analysis is performed, the O3' type crystal structure is preferably 35 wt% or more, more preferably 40 wt% or more, and even more preferably 43 wt% or more.
[0462] The crystallite size of the O3'-type crystal structure of the positive electrode active material is 2 Therefore, even under the same XRD measurement conditions as the positive electrode before and after charging and discharging, the LixCoO 2 When x in the formula is small, a clear peak of the O3' type crystal structure can be confirmed. 2 In this case, even if a part of the crystal structure resembles the O3'-type crystal structure, the crystallite size will be small and the peak will be broad and small. The crystallite size can be determined from the half-width of the XRD peak.
[0463] As described above, the positive electrode active material of one embodiment of the present invention preferably has a small influence of the Jahn-Teller effect. The positive electrode active material of one embodiment of the present invention preferably has a layered rock salt crystal structure and contains cobalt as a transition metal. Furthermore, the positive electrode active material of one embodiment of the present invention may contain the above-described metal Z in addition to cobalt, as long as the influence of the Jahn-Teller effect is small.
[0464] In the positive electrode active material, the range of lattice constants in which the influence of the Jahn-Teller effect is presumed to be small will be considered using XRD analysis.
[0465] FIG. 17 shows the results of estimating the a-axis and c-axis lattice constants using XRD for a positive electrode active material of one embodiment of the present invention having a layered rock-salt crystal structure and containing cobalt and nickel. The positive electrode active material was prepared using steps S11 to S34 described below, with at least a nickel source used in step S21. FIG. 17A shows the a-axis results, and FIG. 17B shows the c-axis results. Note that FIGS. 17A and 17B show the results for the powder of positive electrode active material obtained according to steps S11 to S34. That is, the results are for the powder before being incorporated into a positive electrode. The nickel concentration (%) on the horizontal axis indicates the nickel concentration ratio (proportion) when the sum of the number of cobalt and nickel atoms is taken as 100%. The nickel concentration ratio (proportion) can be determined using a cobalt source and a nickel source.
[0466] FIG. 18 shows the results of estimating the a-axis and c-axis lattice constants using XRD patterns for a positive electrode active material of one embodiment of the present invention having a layered rock-salt crystal structure and containing cobalt and manganese. The positive electrode active material was prepared using steps S11 to S34 described below, with at least a manganese source used in step S21. FIG. 18A shows the a-axis results, and FIG. 18B shows the c-axis results. Note that FIGS. 18A and 18B show the results for the powder of positive electrode active material obtained according to steps S11 to S34. That is, the results are for the material before being incorporated into a positive electrode. The manganese concentration (%) on the horizontal axis represents the concentration ratio (proportion) of manganese when the sum of the number of cobalt and manganese atoms is taken as 100%. The concentration ratio (proportion) of manganese can be determined using a cobalt source and a manganese source.
[0467] Fig. 17C shows the value obtained by dividing the a-axis lattice constant by the c-axis lattice constant (a-axis / c-axis) for the positive electrode active materials whose lattice constant results are shown in Fig. 17A and Fig. 17B. Fig. 18C shows the value obtained by dividing the a-axis lattice constant by the c-axis lattice constant (a-axis / c-axis) for the positive electrode active materials whose lattice constant results are shown in Fig. 18A and Fig. 18B.
[0468] 17C, a significant change in the a-axis / c-axis ratio is observed when the nickel concentration on the horizontal axis is 5% or 7.5%, which suggests that the distortion of the a-axis is large. This distortion may be Jahn-Teller distortion. This suggests that an excellent positive electrode active material with small Jahn-Teller distortion can be obtained when the nickel concentration is less than 7.5%.
[0469] Next, Figure 18A suggests that when the manganese concentration is 5% or more, the behavior of the change in lattice constant is different and does not follow Vegard's law. Therefore, it is suggested that when the manganese concentration is 5% or more, the crystal structure is different. Therefore, the manganese concentration is preferably, for example, 4% or less.
[0470] The above ranges of nickel concentration and manganese concentration do not necessarily apply to the surface layer 115s of the particle, that is, the surface layer 115s of the particle may have higher concentrations than the above ranges.
[0471] As a result of considering a preferable range of the lattice constant from the above, it was found that in the positive electrode active material of one embodiment of the present invention, the a-axis lattice constant is 2.814 × 10 in the layered rock salt crystal structure of the particles of the positive electrode active material in a state where no charge / discharge is performed or in a discharged state, which can be estimated from the XRD pattern. −10 m is greater than 2.817 x 10 −10 m and the lattice constant of the c-axis is 14.05 × 10 −10 m or larger, 14.07 x 10 −10 It has been found that it is preferable that the length be smaller than m. The state in which no charge or discharge is performed may be, for example, the state of powder before the positive electrode of a secondary battery is produced.
[0472] Alternatively, in the layered rock-salt crystal structure of the particles of the positive electrode active material in a state where no charge or discharge is performed or in a discharged state, it is preferable that the value obtained by dividing the lattice constant of the a-axis by the lattice constant of the c-axis (a-axis / c-axis) is greater than 0.20000 and smaller than 0.20049.
[0473] Alternatively, when XRD analysis is performed on a layered rock salt type crystal structure possessed by particles of a positive electrode active material in a state where no charge / discharge is performed or in a discharged state, a first peak may be observed at 2θ of not less than 18.50° and not more than 19.30°, and a second peak may be observed at 2θ of not less than 38.00° and not more than 38.80°.
[0474] The peaks appearing in the powder XRD pattern reflect the crystalline structure of the interior 115c of the positive electrode active material 115, which occupies the majority of the volume of the positive electrode active material 115. The crystalline structure of the surface layer 115s and the like can be analyzed by electron beam diffraction or the like of a cross section of the positive electrode active material 115.
[0475] <XPS> X-ray photoelectron spectroscopy (XPS) can analyze a region from the surface to a depth of 2 nm to 8 nm (usually about 5 nm), so the concentration of each element can be quantitatively analyzed for about half of the surface layer 115s. Furthermore, narrow scan analysis can be used to analyze the bonding state of elements. The quantitative accuracy of XPS is often about ±1 atomic %, and the lower detection limit is about 1 atomic %, depending on the element.
[0476] When the positive electrode active material 115 of one embodiment of the present invention was analyzed by XPS, the number of atoms of the additive element was preferably 1.6 to 6.0 times, and more preferably 1.8 to less than 4.0 times, the number of atoms of the transition metal. When the additive element is magnesium and the transition metal is cobalt, the number of atoms of magnesium is preferably 1.6 to 6.0 times, and more preferably 1.8 to less than 4.0 times, the number of atoms of cobalt. Furthermore, the number of atoms of a halogen such as fluorine is preferably 0.2 to 6.0 times, and more preferably 1.2 to 4.0 times, the number of atoms of the transition metal.
[0477] When XPS analysis is performed, for example, monochromated aluminum can be used as the X-ray source, and the take-off angle can be set to, for example, 45°.
[0478] Furthermore, when the positive electrode active material 115 of one embodiment of the present invention is subjected to XPS analysis, the peak representing the bond energy between fluorine and another element is preferably greater than or equal to 682 eV and less than 685 eV, and more preferably approximately 684.3 eV. This value is different from both the bond energy of lithium fluoride (685 eV) and the bond energy of magnesium fluoride (686 eV). In other words, when the positive electrode active material 115 of one embodiment of the present invention contains fluorine, the bond is preferably other than that of lithium fluoride or magnesium fluoride.
[0479] Furthermore, when the positive electrode active material 115 of one embodiment of the present invention is subjected to XPS analysis, the peak representing the bond energy between magnesium and another element is preferably greater than or equal to 1302 eV and less than 1304 eV, and more preferably about 1303 eV. This value is different from the bond energy of magnesium fluoride, 1305 eV, and is close to the bond energy of magnesium oxide. In other words, when the positive electrode active material 115 of one embodiment of the present invention contains magnesium, the bond is preferably other than that of magnesium fluoride.
[0480] The concentration of added elements, such as magnesium or aluminum, which are preferably present in large amounts in the surface layer 115s, measured by XPS or the like is preferably higher than the concentration measured by ICP-MS (inductively coupled plasma mass spectrometry) or GD-MS (glow discharge mass spectrometry).
[0481] When a cross section of magnesium or aluminum is exposed by processing and analyzed using TEM-EDX, the concentration of the surface layer 115s is preferably higher than the concentration of the inner portion 115c. The processing can be performed using, for example, FIB.
[0482] In an XPS (X-ray photoelectron spectroscopy) analysis, the number of magnesium atoms is preferably 0.4 to 1.5 times the number of cobalt atoms, while in an ICP-MS analysis, the ratio of the number of magnesium atoms, Mg / Co, is preferably 0.001 to 0.06.
[0483] On the other hand, it is preferable that nickel contained in the transition metal is not unevenly distributed in the surface layer portion 115s but is distributed throughout the positive electrode active material 115. However, this does not apply when there is a region where the excess additive element is unevenly distributed as described above.
[0484] <Charge curve and dQ / dV curve> A non-equilibrium phase change occurs around the peak in the dQ / dV curve obtained by differentiating (dQ / dV) the capacity (Q) from the charge curve with respect to the voltage (V), and it is believed that the crystal structure changes significantly. In this specification, a non-equilibrium phase change refers to a phenomenon that causes a non-linear change in a physical quantity.
[0485] FIG. 19 shows charge curves of a secondary battery including a positive electrode active material of one embodiment of the present invention and a secondary battery including a positive electrode active material of a comparative example.
[0486] The positive electrode active material 1 of the present invention shown in FIG. 19 was produced by the production method shown in FIGS. 9A and 9B of the fourth embodiment. More specifically, the LiMO 2 Lithium cobalt oxide (C-10N manufactured by Nippon Chemical Industry Co., Ltd.) was used as the 2 Using this positive electrode active material, a half cell was prepared and charged in the same manner as in the XRD measurement.
[0487] The positive electrode active material 2 of the present invention shown in FIG. 19 was produced by the production method shown in FIGS. 9A and 9C of the fourth embodiment. More specifically, the LiMO 2 Lithium cobalt oxide (C-10N manufactured by Nippon Chemical Industry Co., Ltd.) was used as the 2 , Ni(OH) 2 and Al(OH) 3 Using this positive electrode active material, a half cell was prepared and charged in the same manner as in the XRD measurement.
[0488] 19 was prepared by forming an aluminum-containing layer on the surface of lithium cobalt oxide (C-5H manufactured by Nippon Chemical Industry Co., Ltd.) by a sol-gel method, followed by heating at 500° C. for 2 hours. Using this positive electrode active material, a half cell was prepared and charged in the same manner as in the XRD measurement.
[0489] 19 shows the charging curves when these half-cells were charged at 10 mA / g up to 4.9 V at 25° C. For positive electrode active material 1 and the comparative example, n=2, and for positive electrode active material 2, n=1.
[0490] 20A to 20C show dQ / dV curves, which represent the amount of change in voltage with respect to charge capacity, obtained from the data in Fig. 19. Fig. 20A shows the dQ / dV curve for a half cell using positive electrode active material 1 of one embodiment of the present invention, Fig. 20B shows the dQ / dV curve for a half cell using positive electrode active material 2 of one embodiment of the present invention, and Fig. 20C shows the dQ / dV curve for a half cell using a positive electrode active material of a comparative example.
[0491] As is clear from Figures 20A to 20C, in both the embodiment of the present invention and the comparative example, peaks were observed at voltages of about 4.06 V and about 4.18 V, and the change in capacity with respect to voltage was nonlinear. x CoO 2 It is believed that the crystal structure (space group P2 / m) is when x is 0.5. x CoO 2 In the space group P2 / m where x is 0.5, lithium atoms are aligned as shown in Figure 15. It is thought that energy is consumed for this alignment of lithium atoms, resulting in a nonlinear change in capacity with voltage.
[0492] 20C, large peaks were observed at approximately 4.54 V and 4.61 V. The region between these two peaks is considered to represent an H1-3 phase type crystal structure.
[0493] On the other hand, in the secondary battery of one embodiment of the present invention shown in FIGS. 20A and 20B , which exhibits extremely good cycle characteristics, a small peak was observed at about 4.55 V, but it was not clear. Furthermore, in the case of cathode active material 2, no subsequent peak was observed even above 4.7 V, indicating that the O3′ structure was maintained. As described above, in the dQ / dV curve of a secondary battery using the cathode active material of one embodiment of the present invention, some peaks may be extremely broad or small at 25° C. In such cases, two crystal structures may coexist. For example, two phases, O3 and O3′, or two phases, O3′ and H1-3, may coexist.
[0494] <Discharge Curve and dQ / dV Curve> Furthermore, when the positive electrode active material of one embodiment of the present invention is charged at a high voltage and then discharged at a low rate of, for example, 0.2 C or less, a characteristic voltage change may appear near the end of discharge. This change can be clearly confirmed by the presence of at least one peak in the voltage range up to 3.5 V, which is lower than the peak that appears around 3.9 V, in the dQ / dV curve obtained from the discharge curve.
[0495] <Surface Roughness and Specific Surface Area> The positive electrode active material 115 of one embodiment of the present invention preferably has a smooth surface with few irregularities. A smooth surface with few irregularities is one factor indicating that the distribution of the additive element in the surface layer portion 115s is favorable.
[0496] Whether the surface is smooth and has few irregularities can be determined from, for example, a cross-sectional SEM image or cross-sectional TEM image of the positive electrode active material 115, the specific surface area of the positive electrode active material 115, or the like.
[0497] For example, the surface smoothness can be quantified from a cross-sectional SEM image of the positive electrode active material 115 as follows.
[0498] First, the cathode active material 115 is processed using an FIB or the like to expose a cross section. At this time, it is preferable to cover the cathode active material 115 with a protective film, a protective agent, or the like. Next, an SEM image of the interface between the protective film or the like and the cathode active material 115 is taken. Noise processing is performed on the SEM image using image processing software. For example, Gaussian blurring (σ=2) is performed, followed by binarization. Furthermore, interface extraction is performed using image processing software. Furthermore, the interface line between the protective film or the like and the cathode active material 115 is selected using a magic hand tool or the like, and the data is extracted into a spreadsheet software or the like. Using the functions of the spreadsheet software or the like, correction is performed from a regression curve (quadratic regression), and parameters for roughness calculation are obtained from the data after slope correction, and the root mean square (RMS) surface roughness is calculated by calculating the standard deviation.
[0499] On the particle surfaces of the positive electrode active material 115 of this embodiment, the root mean square (RMS) surface roughness, which is an index of roughness, is preferably 10 nm or less, less than 3 nm, preferably less than 1 nm, and more preferably less than 0.5 nm.
[0500] The image processing software used for noise processing, boundary extraction, etc. is not particularly limited, but for example, "ImageJ" can be used. The spreadsheet software is also not particularly limited, but for example, Microsoft Office Excel can be used.
[0501] For example, the actual specific surface area A measured by the gas adsorption method using the constant volume method R and the ideal specific surface area A i The smoothness of the surface of the positive electrode active material 115 can also be quantified from the ratio of
[0502] Ideal specific surface area A i is calculated assuming that all particles have the same diameter as D50, the same weight, and an ideal spherical shape.
[0503] The median diameter D50 can be measured by a particle size distribution analyzer using a laser diffraction / scattering method, etc. The specific surface area can be measured by a specific surface area measuring device using a gas adsorption method based on a constant volume method, for example.
[0504] The positive electrode active material 115 according to one embodiment of the present invention has an ideal specific surface area A calculated from the median diameter D50. i and the actual specific surface area A R Ratio A R / A i is preferably 2 or less.
[0505] This embodiment can be used in combination with other embodiments.
[0506] [Defects in Positive Electrode Active Material] Examples of defects that may occur in a positive electrode active material are shown in Figures 21 to 31. Note that the positive electrode active material of one embodiment of the present invention is expected to have the effect of suppressing the occurrence of such defects.
[0507] Charging and discharging under high voltage conditions of 4.5 V or higher or at high temperatures (45°C or higher) can cause progressive defects such as pits in the positive electrode active material. Furthermore, cracks can also occur due to the expansion and contraction of the positive electrode active material during charging and discharging. Figure 21 shows a schematic cross-sectional view of a positive electrode active material 51. In the positive electrode active material 51, the pits 54 and 58 are illustrated as holes, but the openings are not circular but have depth. The positive electrode active material 51 may also have cracks 57. The positive electrode active material 51 has crystal faces 55 and may also have recesses 52. Barrier layers 53 and 56 preferably cover the positive electrode active material 51, but may also be separated. The barrier layer 53 also covers the recesses 52.
[0508] The positive electrode active material of a lithium-ion secondary battery is typically LCO or NCM, which can also be considered an alloy containing multiple metal elements (e.g., cobalt, nickel, etc.). At least one of the multiple positive electrode active materials may have defects, and the defects may change before and after charge and discharge. When used in a secondary battery, the positive electrode active material may be chemically or electrochemically eroded by the environmental substances surrounding the positive electrode active material (e.g., electrolyte), or the material may deteriorate. This deterioration does not occur uniformly on the surface of the positive electrode active material, but occurs in a locally concentrated manner, and repeated charge and discharge of the secondary battery may cause defects to form deep from the surface to the interior, for example.
[0509] The phenomenon in which defects progress and form holes in the positive electrode active material may be called pitting corrosion.
[0510] In this specification, cracks and pits are different. Immediately after the preparation of the positive electrode active material, cracks are present but pits are not. Pits are holes formed by the loss of several layers of cobalt or oxygen due to charging and discharging under high voltage conditions of 4.5 V or higher or at high temperatures (45°C or higher), and can also be considered as locations where cobalt has dissolved. Therefore, pits are not present immediately after the preparation of the positive electrode active material. Cracks refer to new surfaces formed by the application of physical pressure or cracks caused by grain boundaries. Cracks may also occur due to particle expansion and contraction caused by charging and discharging. Pits may also occur from cracks or cavities within particles.
[0511] <Disassembly of Secondary Battery> A charge / discharge test was performed up to 50 cycles. The discharge capacity at the 50th cycle was reduced to less than 40% of that at the first cycle. The secondary battery was disassembled, and the positive electrode was removed. Disassembly was performed under an argon atmosphere. After disassembly, the battery was washed with DMC, and the solvent was then evaporated. Observations were made on the positive electrode that had undergone the charge / discharge test up to 50 cycles, and the positive electrode before incorporation into the secondary battery, i.e., the positive electrode immediately after fabrication.
[0512] <SEM Observation> The positive electrode was observed using a scanning electron microscope (SEM). Fig. 22A shows an SEM image of the positive electrode of the secondary battery after 50 cycles. Fig. 22B shows an SEM image of the positive electrode before incorporation into the secondary battery. A scanning electron microscope SU8030 manufactured by Hitachi High-Tech Corporation was used for the SEM observation.
[0513] Next, the cross section of the positive electrode active material was processed using an FIB, and the cross section of the positive electrode active material was observed using an SEM. By repeating the FIB cross section processing and SEM observation, three-dimensional information of the structure as shown in FIG. 23A or 23D can be obtained. Note that a Hitachi High-Tech XVision 210B was used for the FIB processing and SEM observation.
[0514] Fig. 23B is a partially enlarged view of the three-dimensional information in Fig. 23A from the front, and Fig. 23C shows a cross-section of the information sliced across. Fig. 23D corresponds to the three-dimensional information of the side view obtained by rotating the three-dimensional information in Fig. 23A. Fig. 23E is a partially enlarged view of Fig. 23D, and Fig. 23F shows a cross-section of the information sliced across. As shown in Fig. 23F, the pits are not holes, but have a shape that can also be called grooves or fissures that have a width.
[0515] Fig. 24A shows an SEM image of the upper surface of the positive electrode of the secondary battery after 50 cycles. Fig. 24B is a cross-sectional view of the dashed line portion in Fig. 24A. Fig. 24C is an enlarged view of the rectangular framed portion in Fig. 24B. Fig. 24C shows pits 90a, 90b, and 90c.
[0516] Fig. 25A shows an SEM image of the top surface of the positive electrode before it is incorporated into a secondary battery. Fig. 25B is a cross-sectional view of the dashed line portion in Fig. 25A. Fig. 25C is an enlarged view of the rectangular framed portion in Fig. 25B. Fig. 25C shows a crack 91b.
[0517] As described above, when the positive electrode was observed after 50 cycles, pits and cracks were observed.
[0518] <STEM Observation> Next, the cross section of the positive electrode of the secondary battery after 50 cycles was observed by a scanning transmission electron microscope (STEM). The sample for cross section observation was processed using an FIB.
[0519] <EDX Analysis> The positive electrode of the secondary battery after 50 cycles was evaluated using energy dispersive X-ray spectroscopy (EDX).
[0520] Fig. 26A shows a cross-sectional STEM image of the positive electrode, and Fig. 26B is an enlarged view of the area enclosed by the square frame in Fig. 26A.
[0521] EDX mapping of the region shown in FIG. 26B is shown in FIGS. 27A to 27C. FIG. 27A shows EDX mapping of magnesium, FIG. 27B shows EDX mapping of aluminum, and FIG. 27C shows EDX mapping of cobalt. A Hitachi High-Tech HD-2700 was used for the EDX analysis. The acceleration voltage was 200 kV. The EDX mapping suggested that magnesium and aluminum were present in at least a portion of the surface layer of the particles of the positive electrode active material.
[0522] <Micro-electron diffraction> Next, the crystal structure of the grain boundaries of the lithium cobalt oxide and the vicinity thereof was analyzed using micro-electron diffraction.
[0523] Figure 28A is a cross-sectional TEM image of degraded lithium cobalt oxide after 50 cycles. Figure 28B is an enlarged view of the area surrounded by the black line in Figure 28A. The analysis points of the electron microbeam diffraction are indicated by stars NBED1, NBED2, and NBED3 in Figure 28B.
[0524] FIG. 29A shows the electron microbeam diffraction pattern of the star-marked NBED1 portion. The transmitted light is designated O, and some of the diffraction spots are designated DIFF1-1, DIFF1-2, and DIFF1-3, which are shown in the figure. Analysis of the star-marked NBED1 portion revealed that the interplanar spacing of DIFF1-1 was 0.475 nm, the interplanar spacing of DIFF1-2 was 0.199 nm, and the interplanar spacing of DIFF1-3 was 0.238 nm. The plane angles were ∠1O2 = 55°, ∠1O3 = 80°, and ∠2O3 = 24°. The electron beam incident direction was [0-10], and from the interplanar spacing and plane angle, 1 was 10-2 of the layered rock salt crystal, 2 was similarly 10-5, and 3 was similarly 00-3, indicating that LiCoO 2 It was thought to have the following crystal structure.
[0525] Figure 29B shows the electron microbeam diffraction pattern of the star-marked NBED2 portion. The transmitted light is O, and some of the diffraction spots are labeled DIFF2-1, DIFF2-2, and DIFF2-3 in the figure. Analysis of the star-marked NBED2 portion revealed that the interplanar spacing of 1 was 0.468 nm, the interplanar spacing of 2 was 0.398 nm, and the interplanar spacing of 3 was 0.472 nm. The plane angles were ∠1O2 = 54°, ∠1O3 = 110°, and ∠2O3 = 56°. From the interplanar spacings and plane angles, 1, 2, and 3 were spinel-type crystals, and Co 3 O 4 or LiCo 2 O 4 It was thought to have the following crystal structure.
[0526] Figure 29C shows the electron microbeam diffraction pattern of the star NBED3 portion. The transmitted light is O, and some of the diffraction spots are designated DIFF3-1, DIFF3-2, and DIFF3-3, and are shown in the figure. Analysis of the star NBED1 portion revealed that the interplanar spacing of 1 was 0.241 nm, the interplanar spacing of 2 was 0.210 nm, and the interplanar spacing of 3 was 0.246 nm. The plane angles were ∠1O2 = 55 °, ∠1O3 = 110 °, and ∠2O3 = 55 °. Based on the interplanar spacing and plane angles, 1, 2, and 3 were considered to be rock salt crystals with a CoO crystal structure.
[0527] Figure 30A shows a layered rock salt structure, LiCoO 2 The crystal structure of LiCo is shown in FIG. 2 O4 Fig. 30C shows the crystal structure of CoO, which is a rock salt type.
[0528] 31A is a cross-sectional STEM image of a portion of a positive electrode active material layer after a current collector was coated with a slurry that would become the positive electrode active material layer and then pressed. Due to the pressing, steps were observed on the particle surfaces in the direction perpendicular to the lattice fringes (c-axis direction), and evidence of deformation along the lattice fringe direction (the ab-plane direction) was observed.
[0529] 31B is a schematic cross-sectional view of a particle before pressing. In the particle before pressing, a barrier layer is present relatively uniformly on the particle surface in the direction perpendicular to the lattice fringes.
[0530] 31C is a cross-sectional schematic diagram of a particle after pressing. The pressing process causes misalignment in the lattice fringe direction (the ab plane direction). The barrier layer also has multiple steps and is non-uniform. Regarding the misalignment in the ab plane direction, the particle surface opposite to the surface where the irregularities were observed also has irregularities of a similar shape, and some of the particles have misalignment in the ab plane direction.
[0531] The multiple steps shown in Figure 31C are observed as striped patterns on the particle surface. The striped patterns observed on the particle surface due to the steps caused by the displacement caused by pressing are called slips (stacking faults). Such particle slippage can cause the barrier layer to become non-uniform, which can lead to deterioration. Therefore, it is desirable to minimize or eliminate slippage of the positive electrode active material.
[0532] This embodiment mode can be implemented in appropriate combination with other embodiment modes.
[0533] Embodiment Mode 5 In this embodiment mode, examples of various shapes of secondary batteries each having a positive electrode or a negative electrode manufactured by the manufacturing method described in the previous embodiment will be described.
[0534] [Coin-Type Secondary Battery] An example of a coin-type secondary battery will be described. Fig. 32A is an exploded perspective view of a coin-type (single-layer flat) secondary battery, Fig. 32B is an external view, and Fig. 32C is a cross-sectional view thereof. Coin-type secondary batteries are mainly used in small electronic devices. In this specification, coin-type batteries include button-type batteries.
[0535] For ease of understanding, Fig. 32A is a schematic diagram that shows the overlapping of components (upper and lower relationships and positional relationships). Therefore, Fig. 32A and Fig. 32B are not completely identical corresponding views.
[0536] In Fig. 32A, a positive electrode 304, a separator 310, a negative electrode 307, a spacer 322, and a washer 312 are stacked. These are sealed by a negative electrode can 302 and a positive electrode can 301. Note that a gasket for sealing is not shown in Fig. 32A. The spacer 322 and the washer 312 are used to protect the inside or to fix the position inside the can when the positive electrode can 301 and the negative electrode can 302 are crimped together. The spacer 322 and the washer 312 are made of stainless steel or an insulating material.
[0537] A positive electrode 304 has a laminated structure in which a positive electrode active material layer 306 is formed on a positive electrode current collector 305 .
[0538] To prevent short-circuiting between the positive electrode and the negative electrode, a separator 310 and a ring-shaped insulator 313 are arranged so as to cover the side and top surfaces of the positive electrode 304. The separator 310 has a larger planar area than the positive electrode 304.
[0539] FIG. 32B is a perspective view of the completed coin-type secondary battery.
[0540] In the coin-type secondary battery 300, a positive electrode can 301, which also serves as a positive electrode terminal, and a negative electrode can 302, which also serves as a negative electrode terminal, are insulated and sealed by a gasket 303 made of polypropylene or the like. The positive electrode 304 is formed by a positive electrode current collector 305 and a positive electrode active material layer 306 provided in contact with the positive electrode current collector. The negative electrode 307 is formed by a negative electrode current collector 308 and a negative electrode active material layer 309 provided in contact with the negative electrode current collector. The negative electrode 307 is not limited to a laminated structure, and may be formed of lithium metal foil or a lithium-aluminum alloy foil.
[0541] In addition, in each of the positive electrode 304 and the negative electrode 307 used in the coin-type secondary battery 300, the active material layer may be formed only on one surface of the current collector.
[0542] The positive electrode can 301 and the negative electrode can 302 can be made of a metal such as nickel, aluminum, or titanium that is corrosion-resistant to the electrolyte, or an alloy of these metals, or an alloy of these metals with other metals (such as stainless steel). Furthermore, to prevent corrosion by the electrolyte, etc., they are preferably coated with nickel, aluminum, or the like. The positive electrode can 301 is electrically connected to the positive electrode 304, and the negative electrode can 302 is electrically connected to the negative electrode 307.
[0543] These negative electrode 307, positive electrode 304, and separator 310 are immersed in an electrolyte solution, and as shown in FIG. 32C , the positive electrode 304, separator 310, negative electrode 307, and negative electrode can 302 are stacked in this order with the positive electrode can 301 facing downwards, and the positive electrode can 301 and the negative electrode can 302 are crimped together via a gasket 303 to produce a coin-shaped secondary battery 300.
[0544] The coin-type secondary battery 300 has a high capacity, a high discharge capacity, and excellent cycle characteristics. Note that the separator 310 does not need to be provided between the negative electrode 307 and the positive electrode 304.
[0545] [Cylindrical Secondary Battery] An example of a cylindrical secondary battery will be described with reference to Fig. 33A . As shown in Fig. 33A , a cylindrical secondary battery 616 has a positive electrode cap (battery lid) 601 on the top surface and a battery can (external can) 602 on the side and bottom surfaces. The positive electrode cap 601 and the battery can (external can) 602 are insulated by a gasket (insulating packing) 610.
[0546] Fig. 33B is a schematic diagram showing the cross section of a cylindrical secondary battery. The cylindrical secondary battery shown in Fig. 33B has a positive electrode cap (battery lid) 601 on the top surface and a battery can (external can) 602 on the side and bottom surfaces. The positive electrode cap and battery can (external can) 602 are insulated by a gasket (insulating packing) 610.
[0547] A battery element is provided inside a hollow cylindrical battery can 602, which includes a strip-shaped positive electrode 604 and a negative electrode 606 wound with a separator 605 sandwiched between them. Although not shown, the battery element is wound around a central axis. One end of the battery can 602 is closed and the other end is open. The battery can 602 can be made of a metal, such as nickel, aluminum, or titanium, or an alloy of these metals or alloys of these metals with other metals (e.g., stainless steel), which are corrosion-resistant to the electrolyte. To prevent corrosion by the electrolyte, the battery can 602 is preferably coated with nickel, aluminum, or the like. Inside the battery can 602, the wound battery element, which includes the positive electrode, negative electrode, and separator, is sandwiched between a pair of opposing insulating plates 608 and 609. A nonaqueous electrolyte (not shown) is poured into the battery can 602, which contains the battery element. The nonaqueous electrolyte may be the same as that used in coin-type secondary batteries.
[0548] Since the positive and negative electrodes used in a cylindrical storage battery are wound, it is preferable to form active materials on both sides of the current collector. While Figures 33A to 33D illustrate a secondary battery 616 in which the height of the cylinder is greater than the diameter, this is not limiting. A secondary battery in which the diameter of the cylinder is greater than the height of the cylinder may also be used. This configuration, for example, can reduce the size of the secondary battery.
[0549] By using the positive electrode active material 115 obtained in Embodiment 1 for the positive electrode 604, the cylindrical secondary battery 616 can have a large capacity, a large discharge capacity, and excellent cycle characteristics.
[0550] A positive electrode terminal (positive electrode current collector lead) 603 is connected to the positive electrode 604, and a negative electrode terminal (negative electrode current collector lead) 607 is connected to the negative electrode 606. Both the positive electrode terminal 603 and the negative electrode terminal 607 can be made of a metal material such as aluminum. The positive electrode terminal 603 is resistance-welded to a safety valve mechanism 613, and the negative electrode terminal 607 is resistance-welded to the bottom of the battery can 602. The safety valve mechanism 613 is electrically connected to the positive electrode cap 601 via a PTC (Positive Temperature Coefficient) element 611. The safety valve mechanism 613 cuts off the electrical connection between the positive electrode cap 601 and the positive electrode 604 when the increase in internal pressure of the battery exceeds a predetermined threshold. The PTC element 611 is a thermosensitive resistor whose resistance increases as the temperature increases, and the increased resistance limits the amount of current to prevent abnormal heat generation. The PTC element is made of barium titanate (BaTiO 3 )-based semiconductor ceramics, etc. can be used.
[0551] 33C shows an example of a power storage system 615. The power storage system 615 has a plurality of secondary batteries 616. The positive electrodes of each secondary battery are in contact with and electrically connected to conductors 624 separated by insulators 625. The conductors 624 are electrically connected to a control circuit 620 via wiring 623. The negative electrodes of each secondary battery are electrically connected to the control circuit 620 via wiring 626. A protection circuit or the like that prevents overcharging or overdischarging can be used as the control circuit 620.
[0552] 33D shows an example of a power storage system 615. The power storage system 615 has a plurality of secondary batteries 616, which are sandwiched between a conductive plate 628 and a conductive plate 614. The plurality of secondary batteries 616 are electrically connected to the conductive plate 628 and the conductive plate 614 by wiring 627. The plurality of secondary batteries 616 may be connected in parallel, in series, or in parallel and then further connected in series. By configuring the power storage system 615 to have a plurality of secondary batteries 616, a large amount of power can be extracted.
[0553] A plurality of secondary batteries 616 may be connected in parallel and then further connected in series.
[0554] A temperature control device may be provided between the multiple secondary batteries 616. When the secondary batteries 616 are overheated, they can be cooled by the temperature control device, and when the secondary batteries 616 are too cold, they can be heated by the temperature control device. This makes it difficult for the performance of the power storage system 615 to be affected by the outside air temperature.
[0555] 33D , the power storage system 615 is electrically connected to a control circuit 620 via wiring 621 and wiring 622. The wiring 621 is electrically connected to the positive electrodes of the plurality of secondary batteries 616 via a conductive plate 628, and the wiring 622 is electrically connected to the negative electrodes of the plurality of secondary batteries 616 via a conductive plate 614.
[0556] [Another Structural Example of Secondary Battery] Structural examples of secondary batteries will be described with reference to FIGS. 34 and 35. FIG.
[0557] A secondary battery 913 shown in FIG. 34A has a wound body 950 provided with terminals 951 and 952 inside a housing 930. The wound body 950 is immersed in an electrolyte inside the housing 930. The terminal 952 contacts the housing 930, and the terminal 951 is not in contact with the housing 930 by using an insulating material or the like. Note that in FIG. 34A , for convenience, the housing 930 is shown separated, but in reality, the wound body 950 is covered by the housing 930, and the terminals 951 and 952 extend outside the housing 930. The housing 930 can be made of a metal material (such as aluminum) or a resin material.
[0558] 34B, the housing 930 shown in Fig. 34A may be formed from a plurality of materials. For example, the secondary battery 913 shown in Fig. 34B has housings 930a and 930b bonded together, and a wound body 950 is provided in the area surrounded by the housings 930a and 930b.
[0559] The housing 930a can be made of an insulating material such as organic resin. In particular, by using a material such as organic resin on the surface on which the antenna is formed, it is possible to suppress shielding of the electric field by the secondary battery 913. Note that if the shielding of the electric field by the housing 930a is small, the antenna may be provided inside the housing 930a. The housing 930b can be made of, for example, a metal material.
[0560] 34C shows the structure of the wound body 950. The wound body 950 has a negative electrode 931, a positive electrode 932, and a separator 933. The wound body 950 is a wound body in which the negative electrode 931 and the positive electrode 932 are stacked on top of each other with the separator 933 sandwiched therebetween, and the laminated sheet is wound. Note that multiple layers of the negative electrode 931, the positive electrode 932, and the separator 933 may be stacked.
[0561] 35A to 35C may be used as a secondary battery 913 having a wound body 950a. The wound body 950a shown in Fig. 35A has a negative electrode 931, a positive electrode 932, and a separator 933. The negative electrode 931 has a negative electrode active material layer 931a. The positive electrode 932 has a positive electrode active material layer 932a.
[0562] By using the positive electrode active material 115 obtained in Embodiment 1 for the positive electrode 932, the secondary battery 913 can have a large capacity, a large discharge capacity, and excellent cycle characteristics.
[0563] The separator 933 has a width wider than the negative electrode active material layer 931 a and the positive electrode active material layer 932 a, and is wound so as to overlap the negative electrode active material layer 931 a and the positive electrode active material layer 932 a. From the standpoint of safety, it is preferable that the negative electrode active material layer 931 a be wider than the positive electrode active material layer 932 a. A wound body 950 a having such a shape is preferable due to its high safety and productivity.
[0564] 35B, the negative electrode 931 is electrically connected to a terminal 951. The terminal 951 is electrically connected to a terminal 911a. The positive electrode 932 is electrically connected to a terminal 952. The terminal 952 is electrically connected to a terminal 911b.
[0565] 35C , the wound body 950a and the electrolyte are covered by the housing 930 to form the secondary battery 913. It is preferable to provide the housing 930 with a safety valve, an overcurrent protection element, etc. The safety valve is a valve that releases gas when a predetermined pressure is reached inside the housing 930 to prevent the battery from exploding.
[0566] As shown in Fig. 35B, the secondary battery 913 may have multiple wound bodies 950a. Using multiple wound bodies 950a can result in a secondary battery 913 with a larger discharge capacity. For other elements of the secondary battery 913 shown in Figs. 35A and 35B, the descriptions of the secondary battery 913 shown in Figs. 34A to 34C can be referred to.
[0567] 36A and 36B show examples of external views of a laminated secondary battery. Each of the laminated secondary batteries includes a positive electrode 503, a negative electrode 506, a separator 507, an outer casing 509, a positive electrode lead electrode 510, and a negative electrode lead electrode 511.
[0568] FIG. 37A shows the external appearance of a positive electrode 503 and a negative electrode 506. The positive electrode 503 has a positive electrode current collector 501, and a positive electrode active material layer 502 is formed on the surface of the positive electrode current collector 501. The positive electrode 503 also has a region where the positive electrode current collector 501 is partially exposed (hereinafter referred to as a tab region). The negative electrode 506 has a negative electrode current collector 504, and a negative electrode active material layer 505 is formed on the surface of the negative electrode current collector 504. The negative electrode 506 also has a region where the negative electrode current collector 504 is partially exposed, i.e., a tab region. The areas and shapes of the tab regions of the positive electrode and negative electrode are not limited to the example shown in FIG. 37A .
[0569] <Method of Manufacturing Laminated Secondary Battery> Here, an example of a method of manufacturing the laminated secondary battery whose external view is shown in FIG. 36A will be described with reference to FIGS. 37B and 37C.
[0570] First, the negative electrode 506, separator 507, and positive electrode 503 are stacked. Figure 37B shows the stacked negative electrode 506, separator 507, and positive electrode 503. Here, an example is shown in which five pairs of negative electrodes and four pairs of positive electrodes are used. This can also be called a laminate consisting of a negative electrode, a separator, and a positive electrode. Next, the tab regions of the positive electrodes 503 are joined together, and the positive electrode lead electrode 510 is joined to the tab region of the outermost positive electrode. For example, ultrasonic welding or the like may be used for joining. Similarly, the tab regions of the negative electrodes 506 are joined together, and the negative electrode lead electrode 511 is joined to the tab region of the outermost negative electrode.
[0571] Next, the negative electrode 506 , the separator 507 and the positive electrode 503 are arranged on the outer casing 509 .
[0572] Next, as shown in Fig. 37C, the exterior body 509 is folded at the portion indicated by the dashed line. Thereafter, the outer periphery of the exterior body 509 is joined. For example, thermocompression bonding may be used for joining. At this time, an area (hereinafter referred to as an inlet) that is not joined is provided in a part (or one side) of the exterior body 509 so that an electrolyte can be introduced later.
[0573] Next, an electrolyte solution (not shown) is introduced into the inside of the exterior body 509 through an inlet provided in the exterior body 509. The introduction of the electrolyte solution is preferably carried out under a reduced pressure atmosphere or an inert atmosphere. Finally, the inlet is joined. In this manner, the laminated secondary battery 500 can be produced.
[0574] By using the positive electrode active material 115 obtained in Embodiment 1 for the positive electrode 503, the secondary battery 500 can have a large capacity, a high discharge capacity, and excellent cycle characteristics.
[0575] [Example of Battery Pack] An example of a secondary battery pack according to one embodiment of the present invention that can be wirelessly charged using an antenna will be described with reference to FIGS. 38A to 38C.
[0576] Fig. 38A is a diagram showing the appearance of secondary battery pack 531, which has a thin rectangular parallelepiped shape (also called a thick flat plate shape). Fig. 38B is a diagram illustrating the configuration of secondary battery pack 531. Secondary battery pack 531 has circuit board 540 and secondary battery 513. Label 529 is affixed to secondary battery 513. Circuit board 540 is fixed with sticker 515. Secondary battery pack 531 also has antenna 517.
[0577] The inside of the secondary battery 513 may have a structure including a wound body or a laminated body.
[0578] 38B , secondary battery pack 531 has control circuit 590 on circuit board 540. Circuit board 540 is electrically connected to terminal 514. Circuit board 540 is also electrically connected to antenna 517, one 551 of the positive and negative leads of secondary battery 513, and the other 552 of the positive and negative leads.
[0579] Alternatively, as shown in FIG. 38C, the device may have a circuit system 590 a provided on a circuit board 540 and a circuit system 590 b electrically connected to the circuit board 540 via a terminal 514 .
[0580] The antenna 517 is not limited to a coil shape, and may be, for example, a wire shape or a plate shape. Also, antennas such as a planar antenna, an aperture antenna, a traveling wave antenna, an EH antenna, a magnetic field antenna, and a dielectric antenna may be used. Alternatively, the antenna 517 may be a flat conductor. This flat conductor can function as one of the conductors for electric field coupling. In other words, the antenna 517 may function as one of the two conductors of a capacitor. This allows power to be exchanged not only by electromagnetic fields and magnetic fields, but also by electric fields.
[0581] The secondary battery pack 531 has a layer 519 between the antenna 517 and the secondary battery 513. The layer 519 has a function of, for example, shielding an electromagnetic field generated by the secondary battery 513. The layer 519 can be made of, for example, a magnetic material.
[0582] The content of this embodiment mode can be freely combined with the content of other embodiment modes.
[0583] Embodiment 6 In this embodiment, an example of manufacturing an all-solid-state secondary battery using the positive electrode active material 115 obtained in Embodiment 1 will be described.
[0584] As shown in FIG. 39A , a secondary battery 400 of one embodiment of the present invention includes a positive electrode 410 , a solid electrolyte layer 420 , and a negative electrode 430 .
[0585] The positive electrode 410 includes a positive electrode current collector 413 and a positive electrode active material layer 414. The positive electrode active material layer 414 includes a positive electrode active material 411 and a solid electrolyte 421. The positive electrode active material 115 obtained in Embodiment 1 is used for the positive electrode active material 411. The positive electrode active material layer 414 may include a conductive material and a binder.
[0586] Solid electrolyte layer 420 has solid electrolyte 421. Solid electrolyte layer 420 is located between positive electrode 410 and negative electrode 430, and is a region that has neither positive electrode active material 411 nor negative electrode active material 431.
[0587] The negative electrode 430 includes a negative electrode current collector 433 and a negative electrode active material layer 434. The negative electrode active material layer 434 includes a negative electrode active material 431 and a solid electrolyte 421. The negative electrode active material layer 434 may also include a conductive material and a binder. Note that when metallic lithium is used as the negative electrode active material 431, it is not necessary to form the material into particles, and therefore, as shown in FIG. 39B , the negative electrode 430 can be free of the solid electrolyte 421. Using metallic lithium for the negative electrode 430 is preferable because it can improve the energy density of the secondary battery 400.
[0588] As the solid electrolyte 421 included in the solid electrolyte layer 420, for example, a sulfide-based solid electrolyte, an oxide-based solid electrolyte, a halide-based solid electrolyte, or the like can be used.
[0589] The sulfide-based solid electrolytes include thiolithium-based (Li 10 GeP 2 S 12 , Li 3.25 Ge 0.25 P 0.75 S 4etc.), sulfide glass (70Li 2 S・30P 2 S 5 , 30Li 2 S・26B 2 S 3 ・44LiI, 63Li 2 S・36SiS 2 ・1Li 3 P.O. 4 , 57Li 2 S・38SiS 2 ・5Li 4 SiO 4 , 50Li 2 S・50GeS 2 etc.), sulfide crystallized glass (Li 7 P 3 S 11 , Li 3.25 P 0.95 S 4 Sulfide-based solid electrolytes have the advantages of being highly conductive, being able to be synthesized at low temperatures, and being relatively soft, which makes it easy to maintain conductive paths even after charging and discharging.
[0590] The oxide-based solid electrolyte includes a material having a perovskite crystal structure (La 2/3−x Li 3x TiO 3 etc.), materials having a NASICON type crystal structure (Li 1−Y Al Y Ti 2−Y (P.O. 4 ) 3 etc.), materials having a garnet-type crystal structure (Li 7 La 3 Zr 2 O 12 etc.), materials having a LISICON type crystal structure (Li 14 ZnGe 4 O 16 etc.), LLZO (Li 7 La 3 Zr 2 O 12 ), oxide glass (Li 3 P.O. 4 -Li 4 SiO 4 , 50Li 4 SiO 4 ・50Li3 BO 3 etc.), oxide crystallized glass (Li 1.07 Al 0.69 Ti 1.46 (P.O. 4 ) 3 , Li 1.5 Al 0.5 Ge 1.5 (P.O. 4 ) 3 Oxide-based solid electrolytes have the advantage of being stable in the atmosphere.
[0591] Halide-based solid electrolytes include LiAlCl 4 , Li 3 InBr 6 , LiF, LiCl, LiBr, LiI, etc. Composite materials in which these halide-based solid electrolytes are filled into the pores of porous aluminum oxide or porous silica can also be used as the solid electrolyte.
[0592] Also, different solid electrolytes may be mixed and used.
[0593] Among them, Li having a NASICON type crystal structure 1+x Al x Ti 2−x (P.O. 4 ) 3 (0<x<1) (hereinafter, LATP) is preferable because it contains aluminum and titanium, elements that may be contained in the positive electrode active material used in the secondary battery 400 of one embodiment of the present invention, and therefore a synergistic effect can be expected in improving cycle characteristics. In addition, productivity can be expected to be improved by reducing the number of steps. Note that in this specification and the like, the NASICON-type crystal structure refers to a structure having a NASICON-type crystal structure, which is a structure having a NASICON-type crystal structure, and which is ... 2 (XO 4 ) 3 (M: transition metal, X: S, P, As, Mo, W, etc.), and MO 6 Octahedron and XO 4 It refers to a structure in which tetrahedrons are arranged three-dimensionally with their vertices shared.
[0594] [Exterior Body and Shape of Secondary Battery] Various materials and shapes can be used for the exterior body of the secondary battery 400 of one embodiment of the present invention, but it is preferable that the exterior body has a function of applying pressure to the positive electrode, the solid electrolyte layer, and the negative electrode.
[0595] For example, FIG. 40 shows an example of a cell for evaluating materials for an all-solid-state secondary battery.
[0596] 40A is a cross-sectional schematic diagram of the evaluation cell, which has a lower member 761, an upper member 762, and a fixing screw or wing nut 764 that fixes them together, and electrode plate 753 is pressed to fix the evaluation material by rotating a holding screw 763. An insulator 766 is provided between lower member 761 and upper member 762, which are made of stainless steel. An O-ring 765 is also provided between upper member 762 and holding screw 763 to provide a tight seal.
[0597] The evaluation material is placed on electrode plate 751, surrounded by insulating tube 752, and pressed from above by electrode plate 753. Figure 40B is an enlarged perspective view of the evaluation material and its surroundings.
[0598] The evaluation material is an example of a laminate of a positive electrode 750a, a solid electrolyte layer 750b, and a negative electrode 750c, and its cross-sectional view is shown in Fig. 40C. Note that the same reference numerals are used for the same parts in Figs. 40A to 40C.
[0599] The electrode plate 751 and the lower member 761, which are electrically connected to the positive electrode 750a, can be said to correspond to a positive electrode terminal. The electrode plate 753 and the upper member 762, which are electrically connected to the negative electrode 750c, can be said to correspond to a negative electrode terminal. Electrical resistance and the like can be measured by applying pressure to the evaluation material via the electrode plate 751 and the electrode plate 753.
[0600] The secondary battery of one embodiment of the present invention preferably uses an airtight package for its exterior. For example, a ceramic package or a resin package can be used. Furthermore, the exterior is preferably sealed in a sealed atmosphere, such as in a glove box, while blocking external air.
[0601] Fig. 41A shows a perspective view of a secondary battery of one embodiment of the present invention, which has an exterior body and a shape different from those of Fig. 40. The secondary battery in Fig. 41A has external electrodes 771 and 772 and is sealed in an exterior body having a plurality of package members.
[0602] An example of a cross section taken along the dashed line in Figure 41A is shown in Figure 41B. A laminate including a positive electrode 750a, a solid electrolyte layer 750b, and a negative electrode 750c is enclosed and sealed within a package member 770a having a flat plate with an electrode layer 773a, a frame-shaped package member 770b, and a flat plate with an electrode layer 773b. The package members 770a, 770b, and 770c can be made of an insulating material, such as a resin material or ceramic.
[0603] The external electrode 771 is electrically connected to the positive electrode 750a via the electrode layer 773a and functions as a positive electrode terminal, while the external electrode 772 is electrically connected to the negative electrode 750c via the electrode layer 773b and functions as a negative electrode terminal.
[0604] By using the positive electrode active material 115 obtained in Embodiment 1, an all-solid-state secondary battery having high energy density and favorable output characteristics can be realized.
[0605] The content of this embodiment mode can be combined with the content of other embodiment modes as appropriate.
[0606] Seventh Embodiment This embodiment is an example different from the cylindrical secondary battery shown in Fig. 33D. Fig. 42C shows an example of application to an electric vehicle (EV).
[0607] The electric vehicle is equipped with first batteries 1301a and 1301b as main driving secondary batteries, and a second battery 1311 that supplies power to an inverter 1312 that starts a motor 1304. The second battery 1311 is also called a cranking battery or starter battery. The second battery 1311 only needs to have high output, and does not need to have a large capacity, and the capacity of the second battery 1311 is smaller than that of the first batteries 1301a and 1301b.
[0608] The internal structure of the first battery 1301a may be a wound type as shown in Fig. 34A or 35C, or may be a stacked type as shown in Fig. 36A or 36B. The first battery 1301a may use the all-solid-state secondary battery of Embodiment 6. By using the all-solid-state secondary battery of Embodiment 6 for the first battery 1301a, a high capacity can be achieved, safety can be improved, and the battery can be made smaller and lighter.
[0609] In this embodiment, an example is shown in which two first batteries 1301a and 1301b are connected in parallel, but three or more batteries may be connected in parallel. Furthermore, if the first battery 1301a can store sufficient power, the first battery 1301b may be omitted. By configuring a battery pack having multiple secondary batteries, it is possible to extract large amounts of power. The multiple secondary batteries may be connected in parallel, in series, or in series after being connected in parallel. A plurality of secondary batteries is also called a battery pack.
[0610] In addition, in a secondary battery for vehicle use, in order to cut off power from multiple secondary batteries, a service plug or circuit breaker that can cut off high voltage without using tools is provided in the first battery 1301a.
[0611] The power of the first batteries 1301a and 1301b is mainly used to rotate the motor 1304, but also supplies power to 42V in-vehicle components (such as an electric power steering 1307, a heater 1308, and a defogger 1309) via a DCDC circuit 1306. When a rear motor 1317 is provided for the rear wheels, the first battery 1301a is also used to rotate the rear motor 1317.
[0612] In addition, the second battery 1311 supplies power to 14V in-vehicle components (audio 1313, power windows 1314, lamps 1315, etc.) via the DCDC circuit 1310.
[0613] The first battery 1301a will be described with reference to FIG. 42A.
[0614] FIG. 42A shows an example in which nine prismatic secondary batteries 1300 are combined into one battery pack 1415. Furthermore, nine prismatic secondary batteries 1300 are connected in series, with one electrode fixed by a fixing portion 1413 made of an insulator and the other electrode fixed by a fixing portion 1414 made of an insulator. While this embodiment shows an example in which the batteries are fixed by fixing portions 1413 and 1414, they may also be housed in a battery housing box (also called a casing). Because it is expected that a vehicle will be subjected to external vibrations or shaking (such as from the road surface), it is preferable to fix multiple secondary batteries using fixing portions 1413 and 1414 and a battery housing box. Furthermore, one electrode is electrically connected to a control circuit unit 1320 by wiring 1421. The other electrode is electrically connected to the control circuit unit 1320 by wiring 1422.
[0615] A memory circuit including a transistor using an oxide semiconductor may be used for the control circuit portion 1320. A charge control circuit or a battery control system including a memory circuit including a transistor using an oxide semiconductor may be referred to as a battery operating system (BTOS) or a battery oxide semiconductor (BTOS).
[0616] It is preferable to use a metal oxide that functions as an oxide semiconductor. For example, a metal oxide such as In-M-Zn oxide (wherein element M is one or more selected from aluminum, gallium, yttrium, copper, vanadium, beryllium, boron, titanium, iron, nickel, germanium, zirconium, molybdenum, lanthanum, cerium, neodymium, hafnium, tantalum, tungsten, and magnesium) may be used as the oxide. In particular, the In-M-Zn oxide that can be used as the oxide is preferably a C-Axis Aligned Crystal Oxide Semiconductor (CAAC-OS) or a Cloud-Aligned Composite Oxide Semiconductor (CAC-OS). Alternatively, an In—Ga oxide or an In—Zn oxide may be used as the oxide. A CAAC-OS is an oxide semiconductor having multiple crystalline regions, each with its c-axis aligned in a specific direction. The specific direction refers to the thickness direction of the CAAC-OS film, the normal direction to the surface where the CAAC-OS film is formed, or the normal direction to the surface of the CAAC-OS film. A crystalline region is a region with periodic atomic arrangement. If the atomic arrangement is considered as a lattice arrangement, a crystalline region is also a region with a uniform lattice arrangement. Furthermore, a CAAC-OS has a region where multiple crystalline regions are connected in the a-b plane direction, and the region may have distortion. Note that distortion refers to a portion where the lattice arrangement changes between a region with a uniform lattice arrangement and a region with another uniform lattice arrangement in a region where multiple crystalline regions are connected. In other words, a CAAC-OS is an oxide semiconductor with a c-axis aligned and no clear orientation in the a-b plane direction. CAC-OS is a material in which elements constituting a metal oxide are unevenly distributed in a size range of 0.5 nm to 10 nm, preferably 1 nm to 3 nm, or in the vicinity thereof. Note that hereinafter, a state in which one or more metal elements are unevenly distributed in a metal oxide and regions containing the metal elements are mixed in a size range of 0.5 nm to 10 nm, preferably 1 nm to 3 nm, or in the vicinity thereof, is also referred to as a mosaic or patch state.
[0617] Furthermore, the CAC-OS has a mosaic structure in which a material is separated into a first region and a second region, and the first region is distributed throughout the film (hereinafter also referred to as a cloud structure). That is, the CAC-OS is a composite metal oxide having a structure in which the first region and the second region are mixed.
[0618] Here, the atomic ratios of In, Ga, and Zn to the metal elements constituting the CAC-OS in the In—Ga—Zn oxide are denoted as [In], [Ga], and [Zn], respectively. For example, in the CAC-OS in the In—Ga—Zn oxide, the first region is a region where [In] is larger than [In] in the composition of the CAC-OS film. The second region is a region where [Ga] is larger than [Ga] in the composition of the CAC-OS film. Alternatively, for example, the first region is a region where [In] is larger than [In] in the second region and [Ga] is smaller than [Ga] in the second region. The second region is a region where [Ga] is larger than [Ga] in the first region and [In] is smaller than [In] in the first region.
[0619] Specifically, the first region is a region whose main component is indium oxide, indium zinc oxide, or the like. The second region is a region whose main component is gallium oxide, gallium zinc oxide, or the like. In other words, the first region can be referred to as a region whose main component is In. The second region can be referred to as a region whose main component is Ga.
[0620] It should be noted that there are cases where a clear boundary between the first region and the second region cannot be observed.
[0621] For example, in the case of a CAC-OS in an In—Ga—Zn oxide, EDX mapping obtained using energy dispersive X-ray spectroscopy (EDX) can confirm that the CAC-OS has a structure in which a region containing In as a main component (first region) and a region containing Ga as a main component (second region) are unevenly distributed and mixed.
[0622] When a CAC-OS is used in a transistor, the conductivity due to the first region and the insulating property due to the second region act complementarily, thereby providing the CAC-OS with a switching function (a function of turning on / off). That is, a CAC-OS has a conductive function in a part of the material and an insulating function in a part of the material, and functions as a semiconductor as a whole. By separating the conductive function and the insulating function, both functions can be maximized. Therefore, by using a CAC-OS in a transistor, a high on-current (I on ), high field-effect mobility (μ), and good switching behavior can be achieved.
[0623] Oxide semiconductors have a variety of structures, each of which has different characteristics. The oxide semiconductor of one embodiment of the present invention may include two or more of an amorphous oxide semiconductor, a polycrystalline oxide semiconductor, an a-like OS, a CAC-OS, an nc-OS, and a CAAC-OS.
[0624] Furthermore, since the control circuit unit 1320 can be used in high-temperature environments, it is preferable to use a transistor using an oxide semiconductor. To simplify the process, the control circuit unit 1320 may be formed using a unipolar transistor. Transistors using an oxide semiconductor for the semiconductor layer have a wider operating ambient temperature range than single-crystal Si, from −40° C. to 150° C., and their characteristics change less when the secondary battery is heated than single-crystal Si transistors. The off-current of transistors using an oxide semiconductor has low temperature dependence and is below the lower limit of measurement even at 150° C., whereas the off-current characteristics of single-crystal Si transistors are highly temperature dependent. For example, at 150° C., the off-current of a single-crystal Si transistor increases, and the current on / off ratio does not become sufficiently large. The control circuit unit 1320 can improve safety. Furthermore, a synergistic effect on safety can be achieved by combining the positive electrode active material 115 obtained in Embodiment 1 or the like with a secondary battery using the positive electrode.
[0625] The control circuit unit 1320, which uses a memory circuit including transistors using oxide semiconductors, can also function as an automatic control device for a secondary battery to address 10 causes of instability, such as micro-short circuits. The functions for addressing the 10 causes of instability include overcharging prevention, overcurrent prevention, overheating control during charging, cell balancing in the battery pack, over-discharging prevention, a fuel gauge, automatic control of charging voltage and current according to temperature, control of charging current according to the degree of degradation, detection of abnormal behavior of micro-short circuits, and prediction of abnormalities related to micro-short circuits. The control circuit unit 1320 has at least one of these functions. Furthermore, the automatic control device for a secondary battery can be miniaturized.
[0626] A micro-short circuit refers to a tiny short circuit inside a secondary battery, which is not so small that the positive and negative electrodes of the secondary battery are short-circuited and the battery is unable to be charged or discharged, but rather a small short-circuit current flows through the tiny short circuit.Even if the short circuit occurs in a relatively short period of time and in a small location, a large voltage change occurs, and this abnormal voltage value may affect subsequent estimations.
[0627] One of the causes of micro-short circuits is said to be that multiple charge and discharge cycles cause uneven distribution of the positive electrode active material, resulting in localized current concentration in parts of the positive electrode and negative electrode, causing parts of the separator to stop functioning, or the generation of by-products due to side reactions, resulting in micro-short circuits.
[0628] In addition to detecting micro-shorts, the control circuit 1320 can also be said to detect the terminal voltage of the secondary battery and manage the charge / discharge state of the secondary battery. For example, to prevent overcharging, it can turn off both the output transistor and the cutoff switch of the charging circuit almost simultaneously.
[0629] FIG. 42B shows an example of a block diagram of the battery pack 1415 shown in FIG. 42A.
[0630] The control circuit 1320 includes a switch unit 1324 including at least a switch for preventing overcharging and a switch for preventing overdischarging, a control circuit 1322 for controlling the switch unit 1324, and a voltage measurement unit for the first battery 1301a. The control circuit 1320 sets upper and lower voltage limits for the secondary battery used and limits the upper limit of the external current and the upper limit of the output current. The range between the lower and upper voltage limits of the secondary battery is within the recommended voltage range, and when the secondary battery falls outside this range, the switch unit 1324 activates and functions as a protection circuit. The control circuit 1320 can also be called a protection circuit because it controls the switch unit 1324 to prevent overcharging and overdischarging. For example, if the control circuit 1322 detects a voltage that could cause overcharging, it turns off the switch unit 1324 to cut off the current. Furthermore, a PTC element may be provided in the charge / discharge path to provide a function for cutting off the current in response to an increase in temperature. The control circuit section 1320 also has an external terminal 1325 (+IN) and an external terminal 1326 (-IN).
[0631] The switch unit 1324 can be configured by combining n-channel transistors and p-channel transistors. The switch unit 1324 is not limited to a switch having a Si transistor using single crystal silicon, and may be, for example, Ge (germanium), SiGe (silicon germanium), GaAs (gallium arsenide), GaAlAs (gallium aluminum arsenide), InP (indium phosphide), SiC (silicon carbide), ZnSe (zinc selenide), GaN (gallium nitride), GaO xThe switch portion 1324 may be formed using a power transistor having, for example, gallium oxide (x is a real number greater than 0). Furthermore, a memory element using an OS transistor can be freely arranged by stacking it on a circuit using a Si transistor, and therefore integration can be easily achieved. Furthermore, an OS transistor can be manufactured using the same manufacturing equipment as a Si transistor, and therefore can be manufactured at low cost. That is, a control circuit portion 1320 using an OS transistor can be stacked on the switch portion 1324 and integrated into a single chip. The volume occupied by the control circuit portion 1320 can be reduced, enabling miniaturization.
[0632] The first batteries 1301a and 1301b mainly supply power to in-vehicle devices of the 42V system (high voltage system), and the second battery 1311 supplies power to in-vehicle devices of the 14V system (low voltage system).
[0633] In this embodiment, an example in which lithium ion secondary batteries are used for both the first battery 1301a and the second battery 1311 is shown. A lead storage battery, an all-solid-state secondary battery, or an electric double layer capacitor may be used for the second battery 1311. For example, the all-solid-state secondary battery of Embodiment 6 may be used. By using the all-solid-state secondary battery of Embodiment 6 for the second battery 1311, high capacity can be achieved, and reductions in size and weight can be achieved.
[0634] Furthermore, regenerative energy generated by the rotation of the tire 1316 is sent to the motor 1304 via the gear 1305, and is then charged into the second battery 1311 from the motor controller 1303 and the battery controller 1302 via the control circuit unit 1321. Alternatively, the first battery 1301a is charged from the battery controller 1302 via the control circuit unit 1320. Alternatively, the first battery 1301b is charged from the battery controller 1302 via the control circuit unit 1320. In order to efficiently charge the regenerative energy, it is desirable that the first batteries 1301a and 1301b be capable of rapid charging.
[0635] The battery controller 1302 can set the charging voltage and charging current of the first batteries 1301a and 1301b. The battery controller 1302 can set charging conditions in accordance with the charging characteristics of the secondary battery used, and can perform rapid charging.
[0636] Although not shown, when an external charger is connected, the charger's outlet or the charger's connection cable is electrically connected to the battery controller 1302. Power supplied from the external charger is charged to the first batteries 1301a and 1301b via the battery controller 1302. Some chargers are provided with a control circuit, and although the functions of the battery controller 1302 may not be used, it is preferable to charge the first batteries 1301a and 1301b via the control circuit unit 1320 to prevent overcharging. The control circuit unit 1320 may also be provided in the connection cable or the charger's connection cable. The control circuit unit 1320 is sometimes called an ECU (Electronic Control Unit). The ECU is connected to a CAN (Controller Area Network) provided in the electric vehicle. CAN is one of the serial communication standards used as an in-vehicle LAN. The ECU includes a microcomputer. The ECU uses a CPU or a GPU.
[0637] External chargers installed at charging stations and the like come in a variety of types, including 100V outlets, 200V outlets, and three-phase 200V and 50kW outlets. Charging can also be performed by receiving power from external charging equipment using a wireless power supply system or the like.
[0638] When rapid charging is performed, a secondary battery that can withstand high voltage charging is desired in order to charge in a short time.
[0639] The secondary battery of this embodiment uses the positive electrode active material 115 obtained in Embodiment 1 or the like. Furthermore, by using graphene as a conductive material, a secondary battery with significantly improved electrical characteristics can be realized, as a synergistic effect, in which a capacity decrease is suppressed and a high capacity is maintained even when the electrode layer is thickened and the amount of graphene supported is increased. This is particularly effective for a secondary battery used in a vehicle, and a vehicle with a long cruising range, specifically, a cruising distance of 500 km or more per charge, can be provided without increasing the ratio of the weight of the secondary battery to the total weight of the vehicle.
[0640] In particular, the secondary battery of the present embodiment described above can increase the operating voltage of the secondary battery by using the positive electrode active material 115 described in Embodiment 1 etc., and can increase the usable capacity as the charging voltage increases. Furthermore, by using the positive electrode active material 115 described in Embodiment 1 etc. for the positive electrode, a secondary battery for a vehicle having excellent cycle characteristics can be provided.
[0641] Next, an example in which a secondary battery according to one embodiment of the present invention is mounted on a vehicle, typically a transportation vehicle, will be described.
[0642] 33D, 35C, and 42A can be installed in a vehicle to realize next-generation clean energy automobiles, such as hybrid vehicles (HVs), electric vehicles (EVs), and plug-in hybrid vehicles (PHVs). Furthermore, the secondary battery can also be installed in transportation vehicles, such as agricultural machinery, mopeds including electrically assisted bicycles, motorcycles, electric wheelchairs, electric carts, small or large ships, submarines, aircraft such as fixed-wing aircraft and rotary-wing aircraft, rockets, artificial satellites, space probes, planetary probes, and spacecraft. Th...
Claims
1. A secondary battery having a positive electrode and a negative electrode, One or both of the positive electrode and the negative electrode has an active material and a composite compound having a crystal structure, The composite compound functions as a binder and an electrolyte.
2. A secondary battery having a positive electrode and a negative electrode, One or both of the positive electrode and the negative electrode includes an active material, a composite compound having a crystal structure, and a first binder; The composite compound functions as a second binder and an electrolyte.
3. A secondary battery having a positive electrode and a negative electrode, One or both of the positive electrode and the negative electrode has an active material and a composite compound having a crystal structure, The composite compound has a function as a binder, The composite compound includes succinonitrile, lithium ions, and bis(fluorosulfonyl)imide ions.
4. A secondary battery having a positive electrode and a negative electrode, One or both of the positive electrode and the negative electrode has an active material and a composite compound having a crystal structure, The composite compound has a function as a binder, The composite compound includes glutaronitrile, lithium ions, and bis(fluorosulfonyl)imide ions.
5. A secondary battery having a positive electrode and a negative electrode, One or both of the positive electrode and the negative electrode has an active material and a composite compound having a crystal structure, The composite compound has a function as a binder, The composite compound includes adiponitrile, lithium ions, and bis(fluorosulfonyl)imide ions.
6. A secondary battery having a positive electrode, a negative electrode, and an electrolyte, One or both of the positive electrode and the negative electrode has an active material and a composite compound having a crystal structure, The composite compound has a function as a binder, the composite compound has a region located between the active material and the electrolyte, The composite compound includes succinonitrile, lithium ions, and bis(fluorosulfonyl)imide.
7. A secondary battery having a positive electrode, a negative electrode, and an electrolyte, One or both of the positive electrode and the negative electrode has an active material and a composite compound having a crystal structure, The composite compound has a function as a binder, the composite compound has a region located between the active material and the electrolyte, The composite compound includes glutaronitrile, lithium ions, and bis(fluorosulfonyl)imide.
8. A secondary battery having a positive electrode, a negative electrode, and an electrolyte, One or both of the positive electrode and the negative electrode has an active material and a composite compound having a crystal structure, The composite compound has a function as a binder, the composite compound has a region located between the active material and the electrolyte, The composite compound includes adiponitrile, lithium ions, and bis(fluorosulfonyl)imide ions.
9. A secondary battery having a positive electrode and a negative electrode, One or both of the positive electrode and the negative electrode has an active material and a composite compound having a crystal structure, The composite compound has a function as a binder and an electrolyte, The composite compound includes succinonitrile, lithium ions, and bis(fluorosulfonyl)imide ions.
10. A secondary battery having a positive electrode and a negative electrode, One or both of the positive electrode and the negative electrode has an active material and a composite compound having a crystal structure, The composite compound has a function as a binder and an electrolyte, The composite compound includes glutaronitrile, lithium ions, and bis(fluorosulfonyl)imide ions.
11. A secondary battery having a positive electrode and a negative electrode, One or both of the positive electrode and the negative electrode has an active material and a composite compound having a crystal structure, The composite compound has a function as a binder and an electrolyte, The composite compound includes adiponitrile, lithium ions, and bis(fluorosulfonyl)imide.
12. In any one of claims 1 to 11, the positive electrode has an active material including a composite oxide including magnesium and cobalt, the cobalt is present inside and on the surface of the active material; The magnesium is present at least in the surface layer portion.
13. In any one of claims 1 to 12, The secondary battery according to claim 1, wherein the active material of the positive electrode has a surface roughness of at least less than 3 nm when surface unevenness information is quantified in a cross section observed with a scanning transmission electron microscope (STEM).
14. In any one of claims 1 to 13, A secondary battery having a separator between the positive electrode and the negative electrode.
15. In any one of claims 1 to 14, The positive electrode of the secondary battery has an active material having a layered rock salt type crystal structure.
16. In any one of claims 1 to 15, The negative electrode has an active material containing silicon or carbon.
17. In any one of claims 1 to 16, The secondary battery, wherein either or both of the positive electrode and the negative electrode contain a conductive material.
18. In claim 17, The conductive material of the positive electrode comprises carbon black, graphene, or carbon nanotubes.
19. In claim 17 or 18, The conductive material of the negative electrode comprises carbon black, graphene, or carbon nanotubes.
20. 20. An electricity storage system comprising: the secondary battery according to claim 1; and a protection circuit.
21. A vehicle comprising the secondary battery according to any one of claims 1 to 20.
22. A first step and a second step, The first step includes a process of heating a composite compound having a crystalline structure and a positive electrode active material while mixing them to prepare a positive electrode slurry, the second step includes applying the positive electrode slurry to a current collector; The heating is performed at a temperature equal to or higher than the melting point of the complex compound having a crystal structure. How to make the positive electrode.
23. A first step and a second step, The first step includes a process of heating a first compound, a second compound, and a positive electrode active material while mixing them to prepare a positive electrode slurry, the second step includes applying the positive electrode slurry to a current collector; The heating in the first step is carried out at a temperature equal to or higher than the melting points of the first compound and the second compound. How to make the positive electrode.
24. The method includes a first step to a third step, The first step includes a process of heating a first compound and a second compound while mixing them to prepare a composite compound having a crystal structure, The second step includes a process of heating a positive electrode active material and the composite compound while mixing them to prepare a positive electrode slurry, the third step includes applying the positive electrode slurry to a current collector; The heating in the first step is carried out at a temperature equal to or higher than the melting point of the complex compound. How to make the positive electrode.
25. 25. The method according to claim 23 or 24, wherein the first compound comprises succinonitrile, glutaronitrile, or adiponitrile, and the second compound comprises lithium bis(fluorosulfonyl)imide. How to make the positive electrode.
26. The method includes a first step to a fifth step, The first step includes a step of mixing a first binder mixture and a conductive material to prepare a first mixture, The second step includes a step of mixing the first mixture with a positive electrode active material to prepare a second mixture, The third step includes a step of mixing the second mixture, a second binder mixture, and a dispersion medium to prepare a third mixture, the fourth step includes a step of applying the third mixture to a current collector and drying the dispersion medium to prepare a coated electrode; The fifth step includes a step of injecting a composite compound having a crystalline structure into a gap of the coated electrode while heating the composite compound. How to make the positive electrode.
27. In claim 26, the composite compound having a crystal structure is obtained by mixing and heating succinonitrile, glutaronitrile, or adiponitrile with lithium bis(fluorosulfonyl)imide. How to make the positive electrode.