All-solid-state battery
Patent Information
- Application Number
- JP2024502809
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-01
AI Technical Summary
Conventional all-solid-state batteries have low output voltage and low energy density due to their design and materials used.
The development of an all-solid-state battery with a sintered body comprising a positive electrode, a negative electrode, and a solid electrolyte layer, where the negative electrode includes a first solid electrolyte with a γ-Li3PO4 crystal structure and a second solid electrolyte with a similar crystal structure, along with Ag or its alloy, and the positive electrode contains lithium cobalt oxide, enhancing energy density.
The battery achieves high energy density through optimized electrode compositions and structures, particularly with the use of γ-Li3PO4 and Li3+xSi1-xO4 solid electrolytes and Ag or Ag alloy in the negative electrode, resulting in improved output voltage and capacity.
Abstract
Description
all solid state battery
[0001] The present invention relates to an all-solid-state battery. This application claims priority to Japanese Patent Application No. 2022-028957, filed on February 28, 2022, the contents of which are incorporated herein by reference.
[0002] In recent years, electronics technology has made remarkable progress, leading to efforts to make portable electronic devices smaller, lighter, thinner, and more multifunctional. Accordingly, there is a strong demand for batteries that serve as the power source for electronic devices to be smaller, lighter, thinner, and more reliable, and all-solid-state batteries that use solid electrolytes have attracted attention.
[0003] All-solid-state batteries are classified into thin-film and bulk types. Thin-film types are manufactured using thin-film technologies such as physical vapor deposition (PVD) and sol-gel processes. Bulk types are manufactured using powder molding and sintering processes. Each type of all-solid-state battery has different applicable materials and performance due to differences in manufacturing methods.
[0004] For example, Patent Documents 1 and 2 disclose sintered all-solid-state batteries using an oxide-based solid electrolyte as the solid electrolyte, and Patent Documents 1 and 2 describe examples in which titanium oxide is used as the negative electrode active material layer.
[0005] International Publication No. WO 2007 / 135790 International Publication No. WO 2008 / 099508
[0006] The all-solid-state batteries described in Patent Documents 1 and 2 have a small output voltage and a low energy density.
[0007] The present invention has been made in view of the above problems, and has an object to provide an all-solid-state battery with high energy density.
[0008] In order to solve the above problems, the following means are provided.
[0009] (1) A first aspect of the all-solid-state battery includes a sintered body having a positive electrode, a negative electrode, and a solid electrolyte layer between the positive electrode and the negative electrode, and the solid electrolyte layer is made of γ-Li 3 P.O. 4 The negative electrode has a first solid electrolyte having a γ-Li type crystal structure. 3 P.O. 4and at least one selected from Ag and an alloy containing Ag.
[0010] (2) In the all-solid-state battery according to the above aspect, the volume ratio of the second solid electrolyte to the entire negative electrode may be 5% or more and 55% or less.
[0011] (3) In the all-solid-state battery according to the above aspect, the first solid electrolyte is Li 3+x Si x P 1-x O 4 (0.2≦x≦0.6).
[0012] (4) In the all-solid-state battery according to the above aspect, the second solid electrolyte is Li 3+x Si x P 1-x O 4 (0.2≦x≦0.6).
[0013] (5) In the all-solid-state battery according to the above aspect, the first solid electrolyte and the second solid electrolyte may have the same constituent elements.
[0014] (6) In the all-solid-state battery according to the above aspect, a volume ratio of the Ag or Ag alloy to the entire negative electrode may be 45% or more and 95% or less.
[0015] (7) In the all-solid-state battery according to the above aspect, the sum of the volume ratio of the solid electrolyte and the volume ratio of the Ag or Ag alloy to the entire negative electrode may be 95% or more and 100% or less.
[0016] (8) In the all-solid-state battery according to the above aspect, the alloy containing Ag may be a Li—Ag alloy.
[0017] (9) In the all-solid-state battery according to the above aspect, the positive electrode may contain lithium cobalt oxide.
[0018] (10) In the all-solid-state battery according to the above aspect, the positive electrode may include a current collector layer containing Ag and a positive electrode active material layer in contact with at least one main surface of the current collector layer.
[0019] The all-solid-state battery according to the above embodiment has a high energy density.
[0020] Fig. 1 is a cross-sectional view of an all-solid-state battery according to the first embodiment; Fig. 2 is a cross-sectional view showing an enlarged characteristic portion of the all-solid-state battery according to the first embodiment; Fig. 3 is a cross-sectional view showing an enlarged characteristic portion of another example of the all-solid-state battery according to the first embodiment; Fig. 4 is a cross-sectional view showing an enlarged characteristic portion of a positive electrode of another example of the all-solid-state battery according to the first embodiment; Fig. 5 is a cross-sectional view showing an enlarged characteristic portion of a positive electrode of another example of the all-solid-state battery according to the first embodiment.
[0021] The present embodiment will be described in detail below with reference to the accompanying drawings. The drawings used in the following description may show characteristic portions enlarged for the sake of clarity, and the dimensional proportions of each component may differ from the actual proportions. The materials, dimensions, etc. exemplified in the following description are merely examples, and the present invention is not limited thereto. Appropriate modifications may be made within the scope of the present invention.
[0022] The directions are defined as follows. The stacking direction of the laminate 4 is the z direction, one direction in a plane perpendicular to the z direction is the x direction, and the direction perpendicular to the x direction and the z direction is the y direction. Hereinafter, one direction in the z direction may be expressed as "up" and the direction opposite to this direction as "down". Up and down do not necessarily coincide with the direction in which gravity is applied.
[0023] 1 is a cross-sectional schematic diagram of an all-solid-state battery 10 according to this embodiment. The all-solid-state battery 10 has a laminate 4 and terminal electrodes 5 and 6. The terminal electrodes 5 and 6 are in contact with opposing surfaces of the laminate 4. The terminal electrodes 5 and 6 extend in the z direction intersecting (orthogonal to) the laminate surface of the laminate 4.
[0024] The laminate 4 has a positive electrode 1, a negative electrode 2, and a solid electrolyte layer 3. The laminate 4 is a sintered body formed by stacking and sintering the positive electrode 1, the negative electrode 2, and the solid electrolyte layer 3. The number of layers of the positive electrode 1 and the negative electrode 2 is not particularly limited. The solid electrolyte layer 3 is located at least between the positive electrode 1 and the negative electrode 2. Between the positive electrode 1 and the terminal electrode 6 and between the negative electrode 2 and the terminal electrode 5, for example, there is a solid electrolyte identical to the solid electrolyte layer 3. One end of the positive electrode 1 is connected to the terminal electrode 5. One end of the negative electrode 2 is connected to the terminal electrode 6.
[0025] The all-solid-state battery 10 is charged or discharged by the exchange of ions between the positive electrode 1 and the negative electrode 2 via the solid electrolyte layer 3. Although a stacked-type battery is shown in FIG. 1 , a wound-type battery may also be used. The all-solid-state battery 10 is used, for example, in laminated batteries, prismatic batteries, cylindrical batteries, coin-type batteries, button-type batteries, etc. The all-solid-state battery 10 may also be an injection-type battery in which the solid electrolyte layer 3 is dissolved or dispersed in a solvent.
[0026] 2 is an enlarged view of a characteristic portion of the all-solid-state battery 10 according to the first embodiment. The positive electrode 1 has, for example, a positive electrode current collector layer 1A and a positive electrode active material layer 1B. The positive electrode has, for example, a current collector layer containing Ag, and a positive electrode active material layer in contact with at least one main surface of the current collector layer.
[0027] [Positive Electrode Current Collector Layer] The positive electrode current collector layer 1A includes, for example, a current collector 11 and a positive electrode active material 12. In this case, the area between an xy plane passing through the top of the current collector 11 and an xy plane passing through the bottom thereof is regarded as the positive electrode current collector layer 1A.
[0028] The current collector 11 is made of a plurality of current collector particles. The plurality of current collector particles are connected to each other and electrically connected in the xy plane. The positive electrode 1 includes, as the current collector 11, a metal or alloy containing any one selected from the group consisting of Ag, Pd, Au, and Pt. These metals or alloys do not melt even when the laminate 4 is heated in an air atmosphere, and are not easily oxidized. The current collector 11 is, for example, an AgPd alloy, Au, or Pt.
[0029] The positive electrode active material 12 is present in the positive electrode current collector layer 1A together with the current collector 11. The positive electrode active material 12 is in contact with the current collector 11. When the positive electrode current collector layer 1A contains the positive electrode active material 12, electrons are smoothly transferred from the positive electrode active material 12 to the current collector 11. The positive electrode active material 12 is the same as that contained in the positive electrode active material layer 1B described below.
[0030] Although Fig. 2 shows an example in which the current collector 11 is made up of a plurality of current collector particles, the present invention is not limited to this. Fig. 3 is an enlarged view of a characteristic portion of another example of the all-solid-state battery according to the first embodiment. The positive electrode current collector layer 1C shown in Fig. 3 is made up of the current collector 11. The current collector 11 may be in the form of a foil, a punched film, or an expanded material extending in the xy plane.
[0031] The positive electrode active material layer of the positive electrode is in contact with at least one main surface of the current collector layer. The positive electrode active material layer contains a positive electrode active material. The positive electrode active material layer may contain a conductive additive, a binder, and a solid electrolyte described below. The thickness of the positive electrode active material layer may be set within a range of 1 μm to 500 μm.
[0032] [Positive Electrode Active Material Layer] The positive electrode active material layer 1B is formed on one or both surfaces of the positive electrode current collector layer 1A. The positive electrode active material layer 1B contains a positive electrode active material. The positive electrode active material layer 1B may contain a conductive additive, a binder, and the above-mentioned solid electrolyte. When the positive electrode active material layer 1B contains a solid electrolyte, the positive electrode active material layer 1B is considered to be between an xy plane passing through the top of the positive electrode active material and an xy plane passing through the bottom of the positive electrode active material.
[0033] (Positive Electrode Active Material) The positive electrode active material is not particularly limited as long as it can reversibly release and store lithium ions and desorb and insert lithium ions. For example, positive electrode active materials used in known lithium ion secondary batteries can be used.
[0034] The positive electrode active material is, for example, a composite transition metal oxide, a transition metal fluoride, a polyanion, a transition metal sulfide, a transition metal oxyfluoride, a transition metal oxysulfide, or a transition metal oxynitride. The positive electrode active material is preferably a lithium manganese composite oxide, a lithium nickel composite oxide, a lithium cobalt composite oxide, a lithium vanadium composite oxide, a lithium titanium composite oxide, manganese dioxide, titanium oxide, niobium oxide, vanadium oxide, or tungsten oxide. For example, the positive electrode active material is LiCoO 2 , LiMnO 2 and preferably LiCoO 2 These compounds may have deviations from the stoichiometric composition. For example, the positive electrode active material may contain Li x CoO 2 In this case, the lithium cobaltate may be represented by the formula (1), where x varies in the range of 0.4 to 1.2 with the charge and discharge of the all-solid-state battery.
[0035] Furthermore, a positive electrode active material that does not contain lithium can also be used as the positive electrode active material. These positive electrode active materials can be used by disposing metallic lithium or a negative electrode active material doped with lithium ions in the negative electrode in advance, and then starting the battery by discharging. For example, a non-lithium-containing metal oxide (MnO 2 , V 2 O 5 etc.), lithium-free metal sulfides (MoS 2 etc.), lithium-free fluorides (FeF 3 , V.F. 3 ) are examples of these positive electrode active materials.
[0036] (Conductive Aid) The conductive aid is not particularly limited as long as it improves the electronic conductivity in the positive electrode active material layer 1B, and known conductive aids can be used. Examples of the conductive aid include carbon-based materials such as graphite, carbon black, graphene, and carbon nanotubes; metals such as gold, platinum, silver, palladium, aluminum, copper, nickel, stainless steel, and iron; conductive oxides such as ITO; and mixtures thereof. The conductive aid may be in the form of powder or fiber.
[0037] (Binder) The binder bonds the positive electrode current collector layer 1A and the positive electrode active material layer 1B, the positive electrode active material layer 1B and the solid electrolyte layer 3, and the various materials constituting the positive electrode active material layer 1B together.
[0038] The binder can be used within a range that does not impair the function of the positive electrode active material layer 1B. If the binder is not necessary, it does not have to be contained. The content of the binder in the positive electrode active material layer 1B is, for example, 0.5 to 30% by volume of the positive electrode active material layer. If the content of the binder is sufficiently low, the resistance of the positive electrode active material layer 1B becomes sufficiently low.
[0039] The binder may be any material capable of bonding as described above, and examples thereof include fluororesins such as polyvinylidene fluoride (PVDF) and polytetrafluoroethylene (PTFE). Furthermore, in addition to the above, examples of binders that may be used include cellulose, styrene-butadiene rubber, ethylene-propylene rubber, polyimide resin, and polyamide-imide resin. Furthermore, a conductive polymer having electronic conductivity or an ionic conductive polymer having ionic conductivity may be used as the binder. An example of an electrically conductive polymer having electronic conductivity is polyacetylene. In this case, the binder also functions as a conductive additive, so that a conductive additive need not be added. Examples of ionic conductive polymers that may be used include those that conduct lithium ions, and include monomers of polymer compounds (polyether polymer compounds such as polyethylene oxide and polypropylene oxide, polyphosphazene, etc.) and LiClO 4 , LiBF 4 , LiPF 6 Examples of the polymerization initiator used for the complex include a photopolymerization initiator or a thermal polymerization initiator that is compatible with the above-mentioned monomers. The properties required for the binder include oxidation / reduction resistance and good adhesiveness.
[0040] Although specific examples of the positive electrode have been shown so far, the positive electrode is not limited to these examples. For example, Figures 4 and 5 are cross-sectional views of other examples of the positive electrode according to the first embodiment.
[0041] 4 includes a positive electrode current collector layer 1D and a positive electrode active material layer 1B. The positive electrode current collector layer 1D includes a current collector 11, a positive electrode active material 12, and an oxide 13. The oxide 13 is, for example, an oxide containing Ag, such as AgCoO 2 The oxide 13 prevents oxidation of Ag contained in the current collector 11. When the oxide 13 is present between the current collector 11 and the positive electrode active material 12, the cycle characteristics of the all-solid-state battery 10 are improved.
[0042] The positive electrode shown in Fig. 5 has a positive electrode current collector layer 1E, an intermediate layer 1F, and a positive electrode active material layer 1B. The positive electrode current collector layer 1E has a current collector 11 and an oxide 13. The intermediate layer 1F is made of an oxide 13. The example shown in Fig. 5 corresponds to a case where the thickness of the oxide 13 is thicker than the example shown in Fig. 4. The oxide 13 prevents oxidation of Ag contained in the current collector 11, improving the cycle characteristics of the all-solid-state battery 10.
[0043] "Solid Electrolyte Layer" The solid electrolyte layer 3 includes a solid electrolyte. A solid electrolyte is a substance that can move ions by an externally applied electric field. For example, the solid electrolyte layer 3 conducts lithium ions and inhibits the movement of electrons. The solid electrolyte layer 3 is, for example, a sintered body obtained by sintering.
[0044] The solid electrolyte layer 3 is made of γ-Li 3 P.O. 4 The first solid electrolyte includes a first solid electrolyte having a crystalline structure of the Li type. 3+x Si x P 1-x O 4 , Li 3+x Si x V 1-x O 4 , Li 3+x Ge x P 1-x O 4 , Li 3+x Ge x V 1-x O 4 etc. x satisfies 0.2≦x≦0.8. x may also satisfy 0.2≦x≦0.6. The first solid electrolyte may also be a ternary lithium oxide containing Si, V, Ge, and the like.
[0045] "Negative electrode" The negative electrode 2 has, for example, a current collector 21 and a second solid electrolyte 22. In this case, the area between the xy plane passing through the top of the current collector 21 and the xy plane passing through the bottom of the current collector 21 is considered to be the negative electrode 2. The negative electrode 2 may also contain a conductive additive, a binder, etc.
[0046] The current collector 21 is made of one or more materials selected from Ag and alloys containing Ag. Examples of alloys containing Ag include an Ag-Pd alloy and an Ag-Li alloy. When the current collector 21 is an alloy containing Ag, the volume ratio of Ag contained in the alloy is, for example, 80% or more. The current collector 21 may be a foil extending in the xy plane as shown in FIG. 3, or may be in the form of a punched or expanded material.
[0047] Ag and Ag-containing alloys are compounds capable of absorbing and releasing ions. Ag and Ag-containing alloys function as current collectors that conduct electrons toward the terminal electrodes 5 and 6, and as negative electrode active materials that charge and discharge. Therefore, the negative electrode 2 does not need to contain composite transition metal oxides, transition metal fluorides, polyanions, transition metal sulfides, transition metal oxyfluorides, transition metal oxysulfides, transition metal oxynitrides, etc., which generally function as negative electrode active materials. When Ag and Ag-containing alloys with low potential function as the negative electrode 2, the output voltage from the all-solid-state battery 10 increases. The negative electrode 2 may contain only Ag among Ag and Ag-containing alloys. The negative electrode 2 may contain only Ag among Ag and Ag-containing alloys. The negative electrode 2 may contain both Ag and Ag-containing alloys among Ag and Ag-containing alloys.
[0048] Examples of alloys that can be used include Ag--Pd alloys and Ag--Li alloys.
[0049] The volume ratio (first volume ratio) of Ag or an Ag alloy to the entire negative electrode 2 may be 45% or more and 95% or less, 50% or more and 90% or less, 60% or more and 80% or less, or 80% or more.
[0050] The second solid electrolyte 22 is the same as the first solid electrolyte contained in the above-described solid electrolyte layer 3. The volume ratio (second volume ratio) of the second solid electrolyte 22 contained in the negative electrode 2 is, for example, 5% or more. The volume ratio of the second solid electrolyte 22 contained in the negative electrode 2 may be 5% or more and 55% or less, 10% or more and 50% or less, or 20% or more and 40% or less. The first solid electrolyte and the second solid electrolyte 22 may have the same constituent elements.
[0051] The sum of the first volume ratio and the second volume ratio may be 95% or more and 100% or less.
[0052] In the negative electrode 2, the current collector 21 and the second solid electrolyte 22 are in direct contact with each other. The contact rate between the current collector 21 and the second solid electrolyte 22 is, for example, 50% or more, and preferably 80% or more. The contact rate between the current collector 21 and the second solid electrolyte 22 can be determined by extracting any 10 points on the current collector 21 from a cross-sectional image measured with a scanning electron microscope, and dividing the length of the contact portion between the current collector 21 and the second solid electrolyte 22 by the circumferential length of the current collector 21.
[0053] "Method for manufacturing all-solid-state battery" Next, a method for manufacturing the all-solid-state battery 10 will be described. First, the laminate 4 is manufactured. The laminate 4 is manufactured by, for example, a co-firing method or a sequential firing method.
[0054] The co-firing method is a method in which the materials for forming each layer are stacked and then fired all at once to produce the laminate 4. The sequential firing method is a method in which firing is performed after each layer is formed. The co-firing method can produce the laminate 4 with fewer steps than the sequential firing method. Furthermore, the laminate 4 produced by the co-firing method is denser than the laminate 4 produced by the sequential firing method. Below, an example in which the co-firing method is used will be explained.
[0055] First, the materials for the positive electrode current collector layer 1A, the positive electrode active material layer 1B, the solid electrolyte layer 3, and the negative electrode 2 that constitute the laminate 4 are made into a paste. In the example shown in Fig. 4, the current collector 11 is coated with an oxide 13 and then pasted. In the example shown in Fig. 5, the materials for the intermediate layer 1F are also made into a paste.
[0056] The method for forming each material into a paste is not particularly limited, and for example, a method of mixing powders of each material with a vehicle to obtain a paste is used. Here, the vehicle is a general term for a medium in a liquid phase. The vehicle includes a solvent and a binder.
[0057] Next, a green sheet is prepared. The green sheet is obtained by applying a paste prepared for each material onto a substrate such as a PET (polyethylene terephthalate) film, drying it as necessary, and then peeling off the substrate. The method for applying the paste is not particularly limited, and known methods such as screen printing, coating, transfer, and doctor blade can be used.
[0058] Next, the green sheets prepared for each material are stacked in the desired order and in the desired number of layers to prepare a laminate sheet. When stacking the green sheets, alignment and cutting are performed as necessary. For example, when preparing a parallel or series-parallel battery, alignment is performed so that the end face of the positive electrode current collector layer 1A does not coincide with the end face of the negative electrode 2, and then the respective green sheets are stacked.
[0059] The laminate sheet may be fabricated by preparing a positive electrode unit and a negative electrode unit and then laminating these units. The positive electrode unit is a laminate sheet in which a solid electrolyte layer 3, a positive electrode active material layer 1B, a positive electrode current collector layer 1A, and a positive electrode active material layer 1B are laminated in this order. In the example shown in FIG. 5 , an intermediate layer 1F is laminated between the positive electrode current collector layer 1A and the positive electrode active material layer 1B. The negative electrode unit is a laminate sheet in which a solid electrolyte layer 3 and a negative electrode 2 are laminated in this order. The positive electrode unit and the negative electrode unit are laminated so that the solid electrolyte layer 3 of the positive electrode unit and the negative electrode 2 of the negative electrode unit face each other, or so that the positive electrode active material layer 1B of the positive electrode unit and the solid electrolyte layer 3 of the negative electrode unit face each other.
[0060] Next, the produced laminated sheet is pressed together to increase the adhesion of each layer. Pressurization can be performed, for example, by a mold press, hot isostatic pressing (WIP), cold isostatic pressing (CIP), isostatic pressing, or the like. Pressurization is preferably performed while heating. The heating temperature during pressure bonding is, for example, 40 to 95°C. Next, the pressed laminate is cut into chips using a dicing device. The chips are then subjected to a binder removal treatment and sintering to obtain a laminate 4 made of a sintered body.
[0061] The binder removal process can be performed as a separate process from the firing process. By performing the binder removal process, the binder components contained in the chips are thermally decomposed before the firing process, thereby preventing the binder components from rapidly decomposing during the firing process. The binder removal process is performed, for example, by heating in an air atmosphere at a temperature of 300 to 800°C for 0.1 to 10 hours. The atmosphere for the binder removal process is an oxygen partial pressure environment in which the materials constituting the positive electrode, negative electrode, and solid electrolyte do not or are difficult to oxidize and reduce, and the type of gas can be selected arbitrarily so that the materials constituting the positive electrode, negative electrode, and solid electrolyte do not react with the atmospheric gas. For example, the binder removal process may be performed in a nitrogen atmosphere, an argon atmosphere, a nitrogen-hydrogen mixed atmosphere, a water vapor atmosphere, or a mixture thereof.
[0062] The firing step is performed, for example, by placing the chip on a ceramic base. Firing is performed, for example, by heating to 600 to 1000°C in an air atmosphere. The firing time is, for example, 0.1 to 3 hours. The atmosphere for the sintering step is an oxygen partial pressure environment in which the materials constituting the positive electrode, negative electrode, and solid electrolyte do not or do not easily oxidize or reduce, and the type of gas can be selected arbitrarily so that the materials constituting the positive electrode, negative electrode, and solid electrolyte do not react with the atmospheric gas. For example, the sintering step may be performed in a nitrogen atmosphere, an argon atmosphere, a nitrogen-hydrogen mixed atmosphere, a water vapor atmosphere, or an atmosphere containing a mixture of these.
[0063] Alternatively, the sintered laminate 4 (sintered body) may be placed in a cylindrical container together with an abrasive such as alumina and barrel polished. This allows the corners of the laminate to be chamfered. Polishing may also be performed using sandblasting. Sandblasting is preferred because it allows only specific portions to be polished.
[0064] Terminal electrodes 5 and 6 are formed on the opposing side surfaces of the fabricated laminate 4. The terminal electrodes 5 and 6 can be formed by means of sputtering, dipping, screen printing, spray coating, or the like. Through the above-described steps, the all-solid-state battery 10 can be fabricated. When the terminal electrodes 5 and 6 are formed only on predetermined portions, the portions are masked with tape or the like and the above-described process is carried out.
[0065] The all-solid-state battery according to this embodiment has a high energy density. This is because Ag and an alloy containing Ag in the negative electrode 2 function as a negative electrode active material, and the potential of the negative electrode 2 is approximately 0 V (vs. Li + This is thought to be because the potential of the negative electrode 2 is about 0 V and the potential of the negative electrode 3 is about 3.6 V (vs Li + / Li) cathode 1 (LiCoO 2 and LiMn 2 O 4 ) the all-solid-state battery 10 is driven by the potential difference between the electrode 11 and the electrode 12, and the output voltage of the all-solid-state battery increases. The amount of energy of the all-solid-state battery 10 is calculated by multiplying the output voltage of the all-solid-state battery 10 by the capacity of the all-solid-state battery. The energy density of the all-solid-state battery 10 can be compared in terms of the amount of energy if the volume of the all-solid-state battery is the same. Therefore, the all-solid-state battery according to this embodiment has a high energy density.
[0066] The negative electrode 2 is a lithium titanium oxide (potential is about 1.5 V (vs Li + The above output voltage may not be achieved if the negative electrode contains lithium-titanium oxide (Li / Li). The reason for this is unclear, but it is thought that this may be because, depending on the combination of the components that function as the negative electrode active material, lithium-titanium oxide preferentially exchanges lithium ions.
[0067] The above describes the embodiments of the present invention in detail with reference to the drawings. However, each configuration and combination thereof in each embodiment is an example, and additions, omissions, substitutions, and other modifications of the configurations are possible within the scope that does not deviate from the spirit of the present invention.
[0068] "Example 1" (Preparation of Positive Electrode Paste) A positive electrode current collector layer paste was prepared using Ag, Pd, and LiMn 2 O 4 A powder of the above mixed in a volume ratio of 64:16:20 was used. Ethyl cellulose and dihydroterpineol were added to this powder and mixed. Ethyl cellulose was the binder, and dihydroterpineol was the solvent.
[0069] The positive electrode active material layer paste is LiMn 2 O 4 Ethyl cellulose and dihydroterpineol were added to the above mixture and mixed.
[0070] (Preparation of solid electrolyte layer paste) Li 2 CO 3 and SiO 2 and Li 3 P.O. 4 These were used as starting materials and mixed in a molar ratio of 2:1:1. The mixture was wet mixed for 16 hours using a ball mill with water as a dispersion medium. The mixture was calcined at 950°C for 2 hours to obtain Li 3.5 Si 0.5 P 0.5 O 4 Then, 100 parts by mass of this calcined powder, 100 parts by mass of ethanol, and 200 parts by mass of toluene were added to a ball mill and wet mixed. Then, 16 parts by mass of a polyvinyl butyral binder and 4.8 parts by mass of benzyl butyl phthalate were further added and mixed to prepare a solid electrolyte layer paste.
[0071] (Preparation of negative electrode paste) The negative electrode paste is made of Ag, Pd, and Li. 3.5 Si 0.5 P 0.5 O 4 A powder prepared by mixing these in a volume ratio of 76:19:5 was used. Ethyl cellulose and dihydroterpineol were added to this powder and mixed.
[0072] (Fabrication of All-Solid-State Battery) Next, a positive electrode unit and a negative electrode unit were fabricated by the following procedure. First, a positive electrode active material layer paste was printed to a thickness of 5 μm on the above-mentioned solid electrolyte layer sheet using screen printing. Next, the printed positive electrode active material layer paste was dried at 80°C for 5 minutes. Then, a positive electrode current collector layer paste was printed to a thickness of 5 μm on the dried positive electrode active material layer paste using screen printing. Next, the printed positive electrode current collector layer paste was dried at 80°C for 5 minutes. Then, a positive electrode active material layer paste was printed again to a thickness of 5 μm on the dried positive electrode current collector layer paste using screen printing and dried. Then, the PET film was peeled off. In this way, a positive electrode unit was obtained in which a positive electrode active material layer / positive electrode current collector layer / positive electrode active material layer were stacked in this order on the main surface of the solid electrolyte layer.
[0073] Next, a negative electrode paste was printed on the main surface of the solid electrolyte layer to a thickness of 10 μm, and then dried at 80° C. for 5 minutes.
[0074] The laminate was fabricated by stacking five solid electrolyte layer sheets. Fifty electrode units (25 positive electrode units and 25 negative electrode units) were alternately stacked with the solid electrolyte unit sandwiched between them. The units were stacked with each other, with the odd-numbered electrode units extending only to one end face and the even-numbered electrode units extending only to the opposite end face. Six solid electrolyte layer sheets were stacked on top of the stacked units. This was then molded by thermocompression bonding and cut to produce a laminated chip. The laminated chips were then co-fired to obtain a laminate. The co-firing was performed in an air atmosphere, with the temperature rising at a rate of 200°C / hour to a firing temperature of 800°C, and the temperature was maintained for two hours. The unit was then allowed to cool naturally after firing.
[0075] Terminal electrodes 5 and 6 were attached to the sintered laminate (sintered body) by a known method to fabricate an all-solid-state battery. The fabricated all-solid-state battery had the configuration shown in Figure 2. The volume ratio of each layer did not change between the paste state before sintering and the state after sintering. Ag exists either as simple Ag or as an element contained in an AgPd alloy.
[0076] The output voltage and capacity of the fabricated all-solid-state battery were then measured. The capacity is the discharge capacity, and the battery was charged at a constant current of 100 μA (CC charging) until the battery voltage reached 3.9 V in an environment of 60° C., and then discharged at a constant current of 100 μA (CC discharging) until the battery voltage reached 0 V. This cycle was repeated 10 times, and the discharge capacity (μAh) at the 10th cycle was measured. The energy amount (μWh) was then calculated from the product of the output voltage and capacity of the all-solid-state battery.
[0077] "Examples 2 to 5" Examples 2 to 5 are examples of Li when preparing the negative electrode paste. 3.5 Si 0.5 P 0.5 O 4 By changing the amount of Li 3.5 Si 0.5 P 0.5 O 4The other conditions were the same as in Example 1, and measurements similar to those in Example 1 were carried out.
[0078] "Examples 6 to 10" In Examples 6 to 10, the solid electrolyte used in preparing the solid electrolyte layer paste was Li 3.5 Si 0.5 V 0.5 O 4 The solid electrolyte added to the negative electrode paste was changed to Li 3.5 Si 0.5 V 0.5 O 4 The other conditions were the same as in Examples 1 to 5, and measurements similar to those in Examples 1 to 5 were carried out.
[0079] Example 11 In Example 11, a positive electrode current collector layer paste was prepared using Ag, Pd, and LiCoO 2 The positive electrode active material layer paste was made of LiMn 2 O 4 Change to LiCoO 2 The other conditions were the same as in Example 2, and measurements similar to those in Example 2 were carried out.
[0080] Examples 12 to 15 Examples 12 to 15 differ from Example 13 in that the composition ratio of the solid electrolyte used in preparing the solid electrolyte layer paste was changed. 3.6 Si 0.6 P 0.4 O 4 In Example 13, the solid electrolyte was Li 3.4 Si 0.4 P 0.6 O 4 In Example 14, the solid electrolyte was Li 3.2 Si 0.2 P 0.8 O 4 In Example 15, the solid electrolyte was Li 3.1 Si 0.1 P 0.9 O 4 The other conditions were the same as in Example 11, and measurements similar to those in Example 11 were carried out.
[0081] "Example 16" In Example 16, Ag and Li were used when preparing the negative electrode paste. 3.5 Si 0.5 P 0.5 O 4 The powder was mixed in a volume ratio of 80:20, and Ag and LiCoO were used when preparing the positive electrode paste. 2 The difference from Example 11 is that a powder prepared by mixing the above powders in a volume ratio of 80:20 was used. The other conditions were the same as in Example 11, and the same measurements as in Example 11 were carried out.
[0082] "Examples 17 to 23" In Examples 17 to 21, Li was used in the preparation of the negative electrode paste. 3.5 Si 0.5 P 0.5 O 4 By changing the amount of Li 3.5 Si 0.5 P 0.5 O 4 The other conditions were the same as in Example 11, and the same measurements as in Example 11 were carried out. "Example 24" In Example 24, the composition of the solid electrolyte used in preparing the negative electrode paste was changed to Li 3.4 Si 0.4 P 0.6 O 4 This differs from Example 13 in that:
[0083] "Example 25" In Example 25, the solid electrolyte used in preparing the solid electrolyte paste was Li 3.3 Si 0.3 P 0.7 O 4 This differs from Example 29 in that:
[0084] "Example 26" In Example 26, the composition of the solid electrolyte used in preparing the negative electrode paste was changed to Li 3.6 Si 0.6 P 0.4 O 4 This differs from Example 12 in that the above is changed to
[0085] Examples 27 to 30 Examples 27 to 30 differ from Example 11 in that the composition ratio of the solid electrolyte used in preparing the negative electrode paste was changed. In Example 27, the solid electrolyte was Li 3.4 Si 0.4 P0.6 O 4 In Example 28, the solid electrolyte was Li 3.6 Si 0.6 P 0.4 O 4 In Example 29, the solid electrolyte was Li 3.3 Si 0.3 P 0.7 O 4 In Example 30, the solid electrolyte was Li 3.2 Si 0.2 P 0.8 O 4 The other conditions were the same as in Example 11, and measurements similar to those in Example 11 were carried out.
[0086] "Example 31" In Example 31, the solid electrolyte used in preparing the negative electrode paste was Li 3.5 Si 0.5 V 0.5 O 4 The other conditions were the same as in Example 11, and measurements similar to those in Example 11 were carried out.
[0087] In Examples 32 and 33, a Li-Ag alloy was added to the negative electrode current collector layer, and similar studies were conducted. However, the Li-Ag alloy was handled in a glove box with a dew point of -50°C, and the co-firing was carried out by heating the temperature to 800°C at a heating rate of 1200°C / hour in an argon atmosphere, maintaining the temperature for 20 minutes, and then allowing the material to cool naturally after firing. "Examples 32 and 33" In Example 32, when preparing the negative electrode current collector layer, a part of Ag was replaced with a Li-Ag alloy (Li 3.1 The difference from Example 15 is that the amount of Li in the Li-Ag alloy was determined by quantitative analysis using X-ray diffraction (XRD). The other conditions for the measurements were the same as those in Example 1. Example 33 differs from Example 15 in that a part of Ag was replaced with a Li-Ag alloy (Li 4.7 The difference from Example 15 is that the Li content of the Li—Ag alloy was changed to Ag. The Li content of the Li—Ag alloy was determined by quantitative analysis using X-ray diffraction (XRD). The other conditions for the measurements were the same as those for Example 1.
[0088] "Comparative Example 1" In Comparative Example 1, when preparing the negative electrode paste, Li 3.5 Si 0.5 P0.5 O 4 The difference from Example 1 is that no Ag was added. The volume ratio of Ag to Pd was 80:20. The other conditions were the same as in Example 1, and measurements similar to those in Example 1 were carried out.
[0089] "Comparative Example 2" In Comparative Example 2, when preparing the negative electrode paste, Li 3.5 Si 0.5 V 0.5 O 4 The difference from Example 6 is that no Ag was added. The volume ratio of Ag to Pd was 80:20. The other conditions were the same as in Example 6, and measurements similar to those in Example 6 were carried out.
[0090] "Comparative Example 3" In Comparative Example 3, the negative electrode was configured to include a negative electrode current collector layer and a negative electrode active material layer, and this negative electrode unit was laminated on the main surface of the solid electrolyte layer in the following order: negative electrode active material layer / negative electrode current collector layer / negative electrode active material layer. When preparing the paste for the negative electrode current collector layer, powders of Ag and Pd mixed in a volume ratio of 80:20 were used to form an AgPd alloy. The negative electrode active material layer paste contained Li 4 Ti 5 O 12 (Li 4/3 Ti 5/3 O 4 The other conditions were the same as in Example 1, and the same measurements as in Example 1 were carried out.
[0091] "Comparative Example 4" In Comparative Example 4, when preparing the negative electrode paste, Li 3.5 Si 0.5 P 0.5 O 4 Instead of Li 4 Ti 5 O 12 (Li 4/3 Ti 5/3 O 4 The difference from Example 2 is that Ag, Pd, and Li were added. 4/3 Ti 5/3 O 4 The other conditions were the same as in Example 1, and measurements similar to those in Example 1 were carried out.
[0092] Comparative Example 5 Comparative Example 5 differs from Example 2 in that the composition ratio of the solid electrolyte used in preparing the solid electrolyte layer paste was changed. 3.1 Si 0.1 P 0.9 O 4 The solid electrolyte was γ-Li 3 P.O. 4 Instead of the Li type crystal structure, 4 SiO 4 The other conditions were the same as in Example 1, and measurements were carried out in the same manner as in Example 1.
[0093] "Comparative Example 6" In Comparative Example 6, the solid electrolyte layer is Li 4 Ti 5 O 12 γ-Li 3 P.O. 4 This example differs from Example 16 in that the first solid electrolyte does not have the type crystalline structure.
[0094] "Comparative Example 7" In Comparative Example 7, the solid electrolyte contained in the negative electrode was Li 4 Ti 5 O 12 γ-Li 3 P.O. 4 This example differs from Example 16 in that the second solid electrolyte does not have the type crystalline structure.
[0095] "Comparative Example 8" In Comparative Example 8, the negative electrode was configured to include a negative electrode current collector layer and a negative electrode active material layer, and this negative electrode unit was laminated on the main surface of the solid electrolyte layer in the following order: negative electrode active material layer / negative electrode current collector layer / negative electrode active material layer. When preparing the paste for the negative electrode current collector layer, powders of Ag and Pd mixed in a volume ratio of 80:20 were used to form an AgPd alloy. The negative electrode active material layer paste contained Li 4 Ti 5 O 12 (Li 4/3 Ti 5/3 O 4 The other conditions were the same as in Example 16, and the same measurements as in Example 16 were carried out.
[0096] The results of Examples 1 to 33 and Comparative Examples 1 to 8 are summarized in Tables 1 to 3 below.
[0097]
[0098]
[0099] Examples 1 to 33 had a larger amount of output energy than Comparative Examples 1 to 5. Since samples of the same size were prepared for Examples 1 to 33 and Comparative Examples 1 to 8, Examples 1 to 33 had a higher output energy density than Comparative Examples 1 to 8.
[0100] In Comparative Examples 1 and 2, the AgPd alloy functioned as the negative electrode active material, resulting in a large output voltage. On the other hand, in Comparative Examples 1 and 2, the contact area between the solid electrolyte and the AgPd alloy was limited, and sufficient capacity was not obtained. As a result, it is believed that Comparative Examples 1 and 2 did not provide sufficient energy compared to Examples 1 to 14.
[0101] Comparative Examples 3 and 4 show that Li functions as a negative electrode active material. 4/3 Ti 5/3 O 4 is contained in the negative electrode, 4/3 Ti 5/3 O 4 As a result, it is believed that Comparative Examples 3 and 4 did not obtain sufficient amounts of energy compared to Examples 1 to 14.
[0102] In Comparative Example 5, the solid electrolyte layer was γ-Li 3 P.O. 4 Instead of the Li type crystal structure, 4 SiO 4 The crystal structure was of the Li type. 4 SiO 4 The crystal structure of the type is γ-Li 3 P.O. 4 It is believed that the ionic conductivity of Comparative Example 5 is inferior to that of the crystalline structure of the cation exchange type, and sufficient lithium ions cannot be transmitted to the negative electrode, resulting in insufficient capacity. As a result, it is believed that Comparative Example 5 does not provide sufficient energy compared to Examples 1 to 14.
[0103] In Comparative Examples 6 to 8, the solid electrolyte layer was γ-Li 3 P.O. 4 The negative electrode has a first solid electrolyte having a γ-Li type crystal structure. 3 P.O. 4 It is believed that the significant decrease in capacity and energy amount was due to the fact that any one of the following three conditions was not satisfied: that the negative electrode has a second solid electrolyte having a crystalline structure of the above-mentioned type; and that the negative electrode has one or more elements selected from Ag and alloys containing Ag.
[0104] It is possible to provide an all-solid-state battery with a higher energy density than conventional batteries.
[0105] REFERENCE SIGNS LIST 1 Positive electrode 1A, 1C, 1D, 1E Positive electrode current collector layer 1B Positive electrode active material layer 1F Intermediate layer 2 Negative electrode 3 Solid electrolyte layer 4 Laminate 5, 6 Terminal electrode 10 All-solid-state battery 11, 21 Current collector 12 Positive electrode active material 13 Oxide 22 Second solid electrolyte
Claims
1. A sintered body having a positive electrode, a negative electrode, and a solid electrolyte layer between the positive electrode and the negative electrode, The solid electrolyte layer is made of γ-Li 3 P.O. 4 A first solid electrolyte having a crystal structure of the type The negative electrode is γ-Li 3 P.O. 4 and at least one selected from the group consisting of Ag and alloys containing Ag.
2. 2. The all-solid-state battery according to claim 1, wherein a volume ratio of the second solid electrolyte to the entire negative electrode is 5% to 55%.
3. The first solid electrolyte is Li 3+x S x P 1-x O 4 The all-solid-state battery of claim 1 , wherein x is an integer of 0.2 to 0.
6.
4. The second solid electrolyte is Li 3+x S x P 1-x O 4 The all-solid-state battery of claim 1 , wherein x is an integer of 0.2 to 0.
6.
5. The all-solid-state battery according to claim 1 , wherein the first solid electrolyte and the second solid electrolyte have the same constituent elements.
6. 2. The all-solid-state battery in accordance with claim 1, wherein a total volume ratio of the Ag and the alloy containing Ag to the entire negative electrode is 45% or more and 95% or less.
7. 2. The all-solid-state battery according to claim 1, wherein a sum of a volume ratio of the solid electrolyte and a total volume ratio of the Ag and the alloy containing Ag with respect to the entire negative electrode is 95% or more and 100% or less.
8. The all-solid-state battery according to claim 1, wherein the alloy containing Ag is a Li-Ag alloy.
9. The all-solid-state battery according to claim 1 or 2, wherein the positive electrode comprises lithium cobalt oxide.
10. The all-solid-state battery according to claim 8 , wherein the positive electrode comprises: a current collector layer containing Ag; and a positive electrode active material layer in contact with at least one main surface of the current collector layer.