Copper powder and method for producing copper powder

JPWO2023163083A5Pending Publication Date: 2024-11-05
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024503244
Authority / Receiving Office
JP · JP
Patent Type
Applications
Filing Date
2024-08-27
Publication Date
2024-11-05

AI Technical Summary

Technical Problem

Current copper powders for low-temperature sintering in electronic components face challenges such as oxidation, which inhibits sinterability, and require high-vacuum conditions, making them unsuitable for mass production due to the presence of organic components and oxide films that can cause blisters and short circuits.

Method used

A copper powder with an average particle size of 250 nm or less, coated with a specific organic substance formed from a polyol solvent, which prevents the formation of inhibiting oxide films and ensures excellent low-temperature sinterability, achieved by using a polyol method where copper oxide powder is heated in a polyol solvent with a chain organic substance, allowing sintering at lower temperatures without vacuum requirements.

Benefits of technology

The copper powder exhibits excellent oxidation resistance and low-temperature sinterability, preventing oxide film formation that can inhibit sintering, and can be used in mass production without the need for high-vacuum conditions, ensuring stable performance in electronic components like MLCCs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2023163083000001
    Figure 2023163083000001
  • Figure 2023163083000002
    Figure 2023163083000002
  • Figure 2023163083000003
    Figure 2023163083000003
Patent Text Reader

Abstract

Provided is copper powder, which has an average particle size of 250 nm or less and the surface of which is coated with organic matter, wherein the powder satisfies all of conditions (1)-(4) below, is provided with an organic coating film for preventing formation of oxide coating film, which may inhibit sintering, and is excellent in low temperature sinterability. (1) When the organic matter present on the surface of the copper powder is detected by GC / MS analysis, the predetermined organic matter described in the description is detected. (2) When the organic matter present on the surface of the copper powder is detected by LC / MS analysis, the predetermined organic matter described in the description is detected. (3) In the measurement of the heat shrinkage rate of the copper powder green compact, the temperature to give a heat shrinkage rate of 1% is 230°C or less. (4) In the measurement of the heat shrinkage rate of the copper powder green compact, the temperature difference between the temperature to give a heat shrinkage rate of 3% under an inert atmosphere and the temperature to give a heat shrinkage rate of 3% under a reducing atmosphere is less than 10°C.
Need to check novelty before this filing date? Find Prior Art

Description

Copper powder and method for producing copper powder

[0001] The present invention relates to a copper powder obtained by heating a copper oxide powder or copper powder in a polyol solvent, and a method for producing the copper powder.

[0002] Copper powder is also used as a material for conductive pastes to form internal and external electrodes of multilayer ceramic capacitors (MLCCs), which are electronic components, and electrodes of multilayer ceramic substrates. In recent years, as multilayer ceramic capacitors have become smaller and larger in capacity, the internal electrodes have become thinner. For this purpose, fine copper powder is required for the conductive paste (internal electrode paste). Metal microparticles with an average particle size of 250 nm or less, in particular, require a lower firing temperature than typical submicron or larger particles, and are therefore being considered for use in low-temperature firing pastes, etc.

[0003] Furthermore, metal powders that can be sintered at low temperatures not only have less thermal load during sintering and less residual stress during cooling, but also have the advantage of remaining stable once sintered without melting down to the bulk metal melting point. For these reasons, low-temperature sintered metal powders are attracting attention in the fields of printed electronics, which are sensitive to thermal damage to substrates, and die attach for power modules that can operate at high temperatures.

[0004] Currently, nano-sized silver powder is widely used as a low-temperature sintering metal powder, but it has the drawbacks of being expensive and prone to ion migration. Therefore, in recent years, active development has been conducted to develop low-temperature sintering copper powder, which is inexpensive and has excellent resistance to ion migration.

[0005] As with other metal powders, reducing the particle size and increasing the surface energy is effective for low-temperature sintering of copper powder. However, reducing the particle size makes copper powder more susceptible to oxidation, and surface oxidation can actually worsen sinterability. Therefore, an oxidation-resistant film (anti-oxidation film) is required on the surface of copper powder, and this oxidation-resistant film itself must decompose at low temperatures so as not to interfere with sintering.

[0006] That is, for low-temperature sintering of copper powder, two things are essential: the particles must be fine, and the powder must have an oxidation-resistant film that does not inhibit low-temperature sintering.

[0007] In contrast, Patent Document 1 discloses copper powder in which the particle size and particle size distribution are adjusted within a certain range and which combines oxidation resistance and low-temperature sintering by physically adsorbing an aliphatic carboxylic acid having an aliphatic group with five or more carbon atoms onto the surface of the copper particles. According to this document, even when the SEM primary particle size of the copper powder is 100 nm or less, oxidation after standing in air for a long period of time is not confirmed by XRD, and furthermore, it can be sintered at 300°C in a nitrogen atmosphere.

[0008] Patent Document 2 discloses copper powder that can be fired at low temperatures under high vacuum conditions of 0.01 Pa or less by having a cuprous oxide coating on the surface of the copper powder that is controlled to a certain ratio or average coating thickness. According to this document, copper powder in which the cuprous oxide layer coating the copper powder is further protected with caproic acid can be fired at low temperatures under high vacuum conditions of 3×10 -6 Sintering at 100°C was achieved under the condition of Pa.

[0009] In addition to the above-mentioned methods, Patent Document 3 discloses a method (polyol method) in which copper oxide powder (raw material) is heated in a polyol solvent to reduce it. The copper powder produced by this method is characterized by excellent oxidation resistance due to an organic coating formed during reduction. According to this method, by adding a silver salt for nucleation and polyvinylpyrrolidone as a dispersant, copper microparticles with a particle size of 100 nm or less and containing silver as a nucleus can be obtained.

[0010] JP 2016-176146 A International Publication No. 2019 / 106739 A JP 2005-097677 A

[0011] However, the copper powder described in Patent Document 1 contains a large amount of organic components, and is coated with aliphatic carboxylic acids at a high density similar to that of a liquid condensed film. The large amount of organic components present on the copper surface volatilizes during thermal decomposition, generating gas, which may cause defects due to gas generation, such as blistering and short circuits, when forming internal electrodes of MLCCs.

[0012] Furthermore, the copper powder described in Patent Document 3 contains polyvinylpyrrolidone, a high molecular weight polymer, as a dispersant in an amount of 40 mass % relative to the copper.

[0013] Even an extremely thin oxide film formed on the surface of copper powder, a thickness of only a few nanometers, can inhibit sintering. Therefore, although the copper powder described in Patent Document 1 is said to show no XRD peaks derived from oxides immediately after synthesis or after storage in air at 25°C for four months, taking into account the detection sensitivity of XRD, it is difficult to determine the presence or absence of an oxide film large enough to inhibit sintering using XRD.

[0014] Similarly, the copper powder described in Patent Document 2 also has an oxide film formed thereon, which may cause water vapor to be generated as the oxide film is reduced in a reducing atmosphere, or may hinder sintering in an inert atmosphere. Furthermore, high or ultra-high vacuum conditions are required for sintering at the disclosed low temperatures, making it difficult to apply to heating furnaces for mass production, such as conveyor-type continuous heating furnaces.

[0015] The present invention has been made in view of the above-mentioned conventional circumstances, and aims to provide copper powder having an organic coating that prevents the formation of an oxide coating that can inhibit sintering and that has excellent low-temperature sinterability.

[0016] As a result of extensive research aimed at solving the above problems, the present inventors have discovered that by coating the surface of copper powder prepared using a polyol with a mixture of an organic substance derived from the polyol solvent and a chain organic substance having an appropriate molecular weight and functional groups, copper powder can be obtained that has both excellent oxidation resistance and low-temperature sinterability, and have completed the present invention.

[0017] According to an aspect of the present invention, there is provided a copper powder having an average particle size of 250 nm or less and a surface coated with an organic substance, which satisfies all of the following conditions (1) to (4): (1) When the organic substance present on the surface of the copper powder is detected by gas chromatography mass spectrometry (GC / MS), the organic substance is found to be H(—O—CH 2 -CH 2 ) n -OH (where n is an integer of 1 or more and 4 or less), HOOC-CH 2 (-O-CH 2 -CH 2 ) m —OH (where m is an integer of 1 or more and 3 or less), HOOC-CH2 (-O-CH 2 -CH 2 ) l -O-CH 2 -COOH (where l is 1 or 2), H(-C 3 H 6 O) s -OH (where s is an integer of 1 or more and 4 or less), HOOC-CH(CH 3 ) (-C 3 H 6 O) t -OH (where t is an integer of 1 or more and 3 or less), HOOC-CH(CH 3 ) (-C 3 H 6 O) u -O-CH(CH 3 (2) When the organic matter present on the surface of the copper powder is detected by liquid chromatography mass spectrometry (LC / MS), it is found to be a chain organic matter with a molecular weight of 200 to 1000, and the chain organic matter has at each end of the molecule a carboxy group (-COOH), a hydroxy group (-OH), an amino group (-NH 2 ), aldehyde group (-CHO), nitro group (-NO 2 ), thiol group (-SH), sulfo group (-SO 3 HHH), phosphate group (-PO 4 H 2 (3) When a green compact obtained by pressure-molding the copper powder is heated from 25°C in an inert atmosphere, the temperature at which the thermal shrinkage rate reaches 1% is 230°C or less, and (4) when a green compact obtained by pressure-molding the copper powder is heated from 25°C in an inert atmosphere and in a reducing atmosphere, the temperature difference between the temperature at which the thermal shrinkage rate reaches 3% in the inert atmosphere and the temperature at which the thermal shrinkage rate reaches 3% in the reducing atmosphere is less than 10°C, and ...

[0018] According to another aspect of the present invention, there is provided a method for producing copper powder, which comprises mixing copper oxide powder in a polyol solvent having a boiling point of 230°C or less to which the chain organic substance has been added, and heating the resulting copper oxide powder slurry to 230°C or less.

[0019] The amount of the chain organic substance added is preferably 0.005% by mass or more and 10% by mass or less relative to the total amount of copper contained in the copper oxide powder.

[0020] The polyol solvent having a boiling point of 230°C or less is more preferably one or more selected from the group consisting of ethylene glycol (boiling point: 196°C), propylene glycol (boiling point: 188°C), 1,3-propanediol (boiling point: 214°C), 1,2-butanediol (boiling point: 194°C), 1,3-butanediol (boiling point: 207°C), 1,4-butanediol (boiling point: 228°C), 1,2-pentanediol (boiling point: 210°C), and 1,2-hexanediol (boiling point: 223°C).

[0021] According to another aspect of the present invention, there is provided a method for producing copper powder, which comprises dispersing copper powder having an average particle size of 250 nm or less and not satisfying at least one of the conditions (3) and (4) in a polyol solvent having a boiling point of 250°C or higher to which the chain organic substance has been added, to form a copper powder slurry, and then heat-treating the resulting slurry at 230°C or higher.

[0022] Furthermore, it is more preferable that the polyol solvent having a boiling point of 250°C or higher is one or more selected from the group consisting of triethylene glycol (boiling point: 287°C), tetraethylene glycol (boiling point: 327°C), and polyethylene glycol having an average molecular weight of 200 or more and 600 or less (boiling point: around 300°C).

[0023] The temperature of the heat treatment is preferably 230° C. or higher, more preferably 250° C. or higher, and even more preferably 270° C. or higher. The amount of the chain organic substance added is preferably 0.005% by mass or higher and 10% by mass or lower, based on the total amount of copper contained in the copper powder to be heat treated.

[0024] The copper powder according to this embodiment has an organic coating that prevents the formation of an oxide coating that can inhibit sintering, and is a copper powder that has excellent low-temperature sinterability.

[0025] Furthermore, according to the method for producing copper powder according to this embodiment, it is possible to obtain copper powder that has an organic coating that prevents the formation of an oxide coating that can inhibit sintering and that has excellent low-temperature sinterability.

[0026] 1 shows thermomechanical analysis (TMA) profiles of the copper powder prepared in Example 10 under a nitrogen atmosphere and a 2% hydrogen-98% nitrogen atmosphere. FIG. 2 shows the results of gas chromatography mass spectrometry in Example 17 and Conventional Example 3.

[0027] Specific embodiments of the present invention (hereinafter referred to as "present embodiments") will be described in detail below. Note that the present invention is not limited to the following embodiments, and various modifications are possible within the scope of the present invention. In addition, in this specification, the expression "X to Y" (X and Y are arbitrary numerical values) means "X or more and Y or less."

[0028] In the polyol method, when copper oxide powder is suspended in a polyol solvent and heated, the polyol solvent acts as a reducing agent, and reduction to copper powder proceeds. When copper oxide (CuO) is used as the copper oxide powder, copper oxide (CuO) is converted to cuprous oxide (CuO). 2 O) to copper (Cu), which is then converted into copper oxide, 2 When using cuprous oxide (Cu 2 O) is reduced to copper (Cu), and in either case, copper powder (hereinafter, sometimes referred to as "polyol copper powder") is finally obtained. The obtained copper powder is washed with pure water or the like, filtered, and then washed again as necessary and dried. Specifically, one example of washing is a method in which the copper powder (polyol copper powder) obtained by reduction is allowed to settle and decanted, and then pure water or the like is supplied and stirred for washing. One example of filtration is a method in which dehydration is performed by centrifugation.

[0029] The copper powder in this embodiment has an average particle size of 250 nm or less and is surface-coated with an organic substance, and the surface of the copper powder is coated with both a specific organic substance detected by gas chromatography-mass spectrometry (GC / MS) and a specific organic substance detected by liquid chromatography-mass spectrometry (LC / MS). This configuration provides excellent low-temperature sinterability, with a compact obtained by pressing the copper powder and, when heated at a heating rate of 10°C / min based on the thickness of the compact at 25°C, the temperature at which the thermal shrinkage in an inert atmosphere reaches 1% is 230°C or less. Similarly, when a compact obtained by pressing the copper powder and, when heated at a heating rate of 10°C / min based on the thickness of the compact at 25°C, the temperature difference between the temperatures at which the thermal shrinkage in an inert atmosphere reaches 3% and the temperatures at which the thermal shrinkage in a reducing atmosphere reaches 3% is less than 10°C. No oxide coating that could inhibit sintering is formed on the surface of the copper powder, or even if an oxide coating is formed, it is thin enough not to inhibit sintering. The copper powder of this embodiment has an organic coating that prevents the formation of an oxide coating that can inhibit sintering, and is a copper powder with excellent low-temperature sinterability.

[0030] The average particle size of the copper powder is preferably 250 nm or less, more preferably 200 nm or less, and even more preferably 150 nm or less. The average particle size of the copper powder can be, for example, as described in the Examples, and can be 110 nm or less, 100 nm or less, 90 nm or less, 70 nm or less, or 60 nm or less. Because of its fine size, the copper powder can be suitably used for electronic components such as electrodes of multilayer ceramic capacitors. The lower limit of the average particle size of the copper powder is not particularly limited, but the manufacturing method described below sets the lower limit at approximately 20 nm. The average particle size of the copper powder in this embodiment is a value measured by the method described in the Examples. The average particle size of the copper powder can be controlled by the manufacturing conditions, as described later in the manufacturing method section.

[0031] [Gas Chromatography Mass Spectrometry] In the copper powder of this embodiment, the specific organic substance detected by gas chromatography mass spectrometry (GC / MS) is preferably one or more selected from the group consisting of the following organic substances: H(—O—CH 2 -CH 2 )n -OH (where n is an integer of 1 or more and 4 or less), HOOC-CH 2 (-O-CH 2 -CH 2 ) m -OH (where m is an integer of 1 or more and 3 or less), HOOC-CH 2 (-O-CH 2 -CH 2 ) l -O-CH 2 -COOH (where l is 1 or 2), H(-C 3 H 6 O) s -OH (where s is an integer of 1 or more and 4 or less), HOOC-CH(CH 3 ) (-C 3 H 6 O) t -OH (where t is an integer of 1 or more and 3 or less), HOOC-CH(CH 3 ) (-C 3 H 6 O) u -O-CH(CH 3 )-COOH (where u is 1 or 2)

[0032] Among these, it is more preferable to use one or more organic substances selected from the group consisting of organic substances shown in the following (Chemical Formula 1) to (Chemical Formula 8). These organic substances are organic substances derived from polyol solvents. (Chemical Formula 1) Triethylene glycol (H(-O-CH 2 -CH 2 ) 3 —OH) (molecular weight: 150), (chemical formula 2) tetraethylene glycol (H(—O—CH 2 -CH 2 ) 4 —OH) (molecular weight: 194), (Chemical formula 3) 2-[2-(2-hydroxyethoxy)ethoxy]acetic acid (HOOC-CH 2 (-O-CH 2 -CH 2 ) 2 —OH) (molecular weight: 164), (Chemical formula 4) 2-[2-[2-(2-hydroxyethoxy)ethoxy]ethoxy]acetic acid (HOOC-CH 2 (-O-CH 2 -CH 2 ) 3—OH) (molecular weight: 208), (Chemical formula 5) ethylenedioxydiacetic acid (HOOC-CH 2 -O-CH 2 -CH 2 -O-CH 2 —COOH) (molecular weight: 178), (Chemical Formula 6) [oxybis(ethyleneoxy)]diacetic acid (HOOC-CH 2 (-O-CH 2 -CH 2 ) 2 -O-CH 2 —COOH) (molecular weight: 222), (Chemical formula 7) tripropylene glycol (H(—C 3 H 6 O) 3 —OH) (molecular weight: 192, atactic polymer, isotactic polymer, or syndiotactic polymer), (Chemical Formula 8) tetrapropylene glycol (H(—C 3 H 6 O) 4 —OH) (molecular weight: 250, either atactic polymer, isotactic polymer, or syndiotactic polymer). GC / MS is a measurement technique that gasifies and detects organic substances, so the specific organic substances detected by GC / MS can be said to be organic substances that have a relatively small molecular weight and are easily gasified. The method for detecting the organic substances by GC / MS in this embodiment is the same as the method described in the Examples. The structures of the organic substances (Chemical Formula 1) to (Chemical Formula 8) are shown below.

[0033]

[0034] [Liquid Chromatography Mass Spectrometry] Specific organic substances detected by liquid chromatography mass spectrometry (LC / MS) are chain organic substances with a molecular weight of 200 to 1000, and the chain organic substances have functional groups capable of coordinating to copper ions, such as a carboxyl group (—COOH), a hydroxyl group (—OH), and an amino group (—NH), at the ends of their molecules. 2 ), aldehyde group (-CHO), nitro group (-NO2 ), thiol group (-SH), sulfo group (-SO 3 HHH), phosphate group (-PO 4 H 2 ), a cyan group (—CN), a chloro group (—Cl), a bromo group (—Br), and an iodo group (—I).

[0035] Among these, a chain organic substance having a molecular weight of 200 to 700 is more preferred. Furthermore, the chain organic substance preferably has a carboxyl group or a hydroxyl group at each end of the molecule, and more preferably has a carboxyl group or a hydroxyl group at both ends. Examples of such chain organic substances include (Chemical Formula 9) sebacic acid (molecular weight: 202), (Chemical Formula 10) dodecanedioic acid (molecular weight: 230), (Chemical Formula 11) tetradecanedioic acid (molecular weight: 258), (Chemical Formula 12) hexadecanedioic acid (molecular weight: 286), (Chemical Formula 13) octadecanedioic acid (molecular weight: 314), (Chemical Formula 14) eicosanedioic acid (molecular weight: 342), (Chemical Formula 15) poly(ethylene glycol) bis(carboxymethyl) ether (average molecular weight: 250), and (Chemical Formula 16) poly(ethylene glycol) bis(carboxymethyl) ether (average molecular weight: 600). These are also preferred because they are readily available for purchase. The structures of the above organic compounds (Chemical Formula 9) to (Chemical Formula 16) are shown below.

[0036]

[0037] The mechanism by which the copper powder of this embodiment has the low-temperature sinterability described above has not been elucidated in detail, but the specific organic substances detected by GC / MS and the specific organic substances detected by LC / MS have long chain molecules with a small proportion of functional groups capable of coordinating to copper ions. Therefore, even if the copper powder surface is evenly coated with the organic substance, the density of bonds with the copper powder surface via functional groups may be low, making it easier for the organic substance to detach from the copper powder surface due to heat.

[0038] The organic substances detected by the GC / MS may be detected by the LC / MS, and the organic substances detected by the LC / MS may be detected by the GC / MS.

[0039] The copper powder of this embodiment is pressed at 100 MPa to form a green compact, which is then heated in an inert atmosphere from 25°C at a heating rate of 10°C / min. When the thermal shrinkage is measured based on the thickness of the green compact at 25°C, the temperature at which the thermal shrinkage reaches 1% is 230°C or lower. The temperature at which the thermal shrinkage of the green compact reaches 1% is the temperature at which the copper powder begins to shrink in volume due to a sintering phenomenon, and can also be expressed as the temperature at which sintering begins. For example, for the copper powder of this embodiment, the temperature at which the thermal shrinkage reaches 1% can be 220°C or lower, 215°C or lower, 210°C or lower, 205°C or lower, 200°C or lower, 195°C or lower, etc., as described in the examples.

[0040] Furthermore, when the copper powder in this embodiment is compacted under a pressure of 100 MPa to form a powder compact, and heated from 25°C at a heating rate of 10°C / min under an inert atmosphere and a reducing atmosphere, the thermal shrinkage is measured based on the thickness of the powder compact at 25°C. The temperature difference between the temperature at which the thermal shrinkage is 3% under an inert atmosphere and the temperature at which the thermal shrinkage is 3% under a reducing atmosphere is less than 10°C. Since the sintering behavior does not change significantly between the inert and reducing atmospheres used for firing (heating), the constraints imposed by the difficulty of sintering the copper powder are alleviated when selecting a firing atmosphere. The temperature at which the thermal shrinkage of the powder compact is 3% is the temperature at which volumetric shrinkage due to the sintering phenomenon of the copper powder has progressed to a certain extent. This temperature not only serves as an indicator of the sinterability of the copper powder, but also allows the presence or absence of an oxide film that inhibits sintering to be estimated by comparing the temperature measured under an inert atmosphere with that measured under a reducing atmosphere. That is, the temperature difference between the temperatures at which the thermal shrinkage of the green compact becomes 3% in an inert atmosphere and in a reducing atmosphere being less than 10°C means that no oxide film that can inhibit sintering is formed on the surface of the copper powder. For example, in the copper powder of this embodiment, the temperature difference between the temperature at which the thermal shrinkage becomes 3% in an inert atmosphere and the temperature at which the thermal shrinkage becomes 3% in a reducing atmosphere can be 8°C or less, 6°C or less, 5°C or less, etc., as described in the examples.

[0041] Specifically, when the temperature at which the thermal shrinkage of a compact in a reducing atmosphere is 3% is 10°C or more lower than the temperature at which the thermal shrinkage of a compact in an inert atmosphere is 3%, it is thought that the surface of the copper powder used for thermal shrinkage measurement was covered with a thin oxide film, and the oxide film was reduced by the reducing gas, making it easier to sinter (the oxide film inhibited sintering in an inert atmosphere). On the other hand, when the thermal shrinkage of a compact in a reducing atmosphere is measured under conditions where the copper powder used for thermomechanical analysis has a higher oxide content on its surface, a larger amount of water vapor is generated by reduction, and the expansion of the compact due to water vapor exceeds the contraction due to sintering of the copper powder, resulting in a tendency for the thermal shrinkage behavior in the thermomechanical analysis profile to shift toward higher temperatures. This corresponds to a case where the temperature at which the thermal shrinkage of a compact in a reducing atmosphere is 10°C or more higher than the temperature at which the thermal shrinkage of a compact in an inert atmosphere is 3%.

[0042] Although the mechanism by which the copper powder in this embodiment has the effect of preventing the formation of the oxide film described above has not been elucidated in detail, the specific organic substances detected by the GC / MS and the specific organic substances detected by the LC / MS are a combination of organic substances with different molecular lengths, and can efficiently and evenly coat the surface of the copper powder, so it is thought that they may have a high function as an antioxidant film.

[0043] In addition, the organic matter present on the surface of the copper powder in this embodiment, the organic matter detected by the GC / MS, and the organic matter detected by the LC / MS may all contain other substances such as other organic matter or compounds, as long as they do not deviate from the spirit of the present invention.

[0044] As described above, the copper powder of this embodiment has an average particle size of 250 nm or less, and is a copper powder whose surface is coated with an organic substance, and satisfies all of the following conditions (1) to (4): (1) When the organic substance present on the surface of the copper powder is detected by gas chromatography mass spectrometry, the organic substance is H(—O—CH 2 -CH 2 ) n -OH (where n is an integer of 1 or more and 4 or less), HOOC-CH 2 (-O-CH 2 -CH 2 ) m -OH (where m is an integer of 1 or more and 3 or less), HOOC-CH 2 (-O-CH 2 -CH 2 ) l -O-CH 2 -COOH (where l is 1 or 2), H(-C 3 H 6 O) s -OH (where s is an integer of 1 or more and 4 or less), HOOC-CH(CH 3 ) (-C 3 H 6 O) t -OH (where t is an integer of 1 or more and 3 or less), HOOC-CH(CH 3 ) (-C 3 H 6 O) u -O-CH(CH 3(2) When the organic matter present on the surface of the copper powder is detected by liquid chromatography mass spectrometry, it is found to be a chain organic matter with a molecular weight of 200 to 1000, and the chain organic matter has at each end of the molecule a carboxy group (-COOH), a hydroxy group (-OH), an amino group (-NH 2 ), aldehyde group (-CHO), nitro group (-NO 2 ), thiol group (-SH), sulfo group (-SO 3 HHH), phosphate group (-PO 4 H 2 (3) When a green compact obtained by pressure-molding the copper powder is heated from 25°C in an inert atmosphere, the temperature at which the thermal shrinkage becomes 1% is 230°C or less, and (4) when a green compact obtained by pressure-molding the copper powder is heated from 25°C in an inert atmosphere and in a reducing atmosphere, the temperature difference between the temperature at which the thermal shrinkage becomes 3% in the inert atmosphere and the temperature at which the thermal shrinkage becomes 3% in the reducing atmosphere is less than 10°C, and ...

[0045] In the copper powder of this embodiment, the components other than those described above are optional. The copper powder of this embodiment has an organic coating that prevents the formation of an oxide coating that can inhibit sintering, and is a copper powder with excellent low-temperature sinterability.

[0046] Next, the copper powder manufacturing methods (copper powder manufacturing method 1, copper powder manufacturing method 2) according to the present embodiment will be described. In the following description, matters already described may be omitted or simplified. Furthermore, the matters described in the copper powder according to the present embodiment can be applied as appropriate to the copper powder manufacturing method according to the present embodiment. Furthermore, the matters described in the copper powder manufacturing method according to the present embodiment can be applied as appropriate to the copper powder according to the present embodiment.

[0047] (Method 1 for Producing Copper Powder) The method for producing copper powder in this embodiment involves reducing copper oxide powder (raw material) in a polyol solvent having a boiling point of 230°C or less (hereinafter, a polyol solvent having a boiling point of 230°C or less may be referred to as polyol solvent A) to obtain copper powder. In the reduction step, the specific chain organic substance described above is added to polyol solvent A in which copper oxide powder has been suspended (hereinafter, the liquid in which this polyol solvent A and copper oxide powder are mixed and suspended may be collectively referred to as the reaction liquid), and the target copper powder is obtained by heating and reducing. The reduction step allows an organic substance containing the added chain organic substance to be applied to the surface of the copper powder, thereby obtaining the copper powder of this embodiment described above.

[0048] The chain organic substance to be added may be in the form of a salt or the like, as long as it is in the form of the chain organic substance in the reaction liquid.

[0049] The copper oxide powder used as a raw material in the reduction process is copper oxide (CuO), cuprous oxide (Cu 2 The copper oxide powder may be crushed in advance before being subjected to the reduction reaction.

[0050] The polyol solvent A used in the reduction step is a polyol solvent having a boiling point of 230°C or less, and is more preferably one or more selected from the group consisting of ethylene glycol (boiling point: 196°C), propylene glycol (boiling point: 188°C), 1,3-propanediol (boiling point: 214°C), 1,2-butanediol (boiling point: 194°C), 1,3-butanediol (boiling point: 207°C), 1,4-butanediol (boiling point: 228°C), 1,2-pentanediol (boiling point: 210°C), and 1,2-hexanediol (boiling point: 223°C). The amount of the chain organic substance added to polyol solvent A is preferably 0.005% by mass or more and 10% by mass or less, based on the total amount of copper contained in the copper oxide powder.

[0051] The reaction temperature in the reduction step is preferably −50° C. or higher relative to the boiling point of polyol solvent A, and more preferably −40° C. or higher relative to the boiling point of polyol solvent A. The reaction temperature is preferably ±0° C. or lower relative to the boiling point of polyol solvent A, and more preferably −5° C. or lower relative to the boiling point of polyol solvent A. The reaction temperature is preferably −50° C. or higher relative to the boiling point of polyol solvent A and ±0° C. or lower relative to the boiling point of polyol solvent A, and more preferably −40° C. or higher relative to the boiling point of polyol solvent A and −5° C. or lower relative to the boiling point of polyol solvent A. If the reaction temperature is set to a temperature lower than −50° C. relative to the boiling point of polyol solvent A, the reduction reaction may not proceed sufficiently, resulting in residual copper oxide powder (raw material), which may increase the oxygen content in the resulting copper powder (polyol copper powder), and the reaction time may be significantly extended, resulting in reduced productivity. Furthermore, if the heating temperature is set higher than the boiling point of the polyol solvent A, the polyol solvent will be significantly reduced (consumed) due to decomposition and volatilization, and there is a risk that sufficient reduction will not be achieved.

[0052] In the reduction step, copper oxide powder is heated and reduced in polyol solvent A to which the chain organic substance has been added to obtain copper powder according to this embodiment. In the reduction reaction, heating is started after the chain organic substance has been added to the reaction solution. However, the chain organic substance may also be added later to the reaction solution while the temperature is being increased.

[0053] When using a chain organic substance that does not become neutral (pH of about 6.5 to 7.5) when made into an aqueous solution, it is preferable to add an alkali or acid as a neutralizing agent to neutralize the chain organic substance added to the reaction solution. When using an alkali as the neutralizing agent, an alkali metal hydroxide is preferred, and specifically, sodium hydroxide or potassium hydroxide can be used. When using an acid as the neutralizing agent, an inorganic acid is preferred, and specifically, sulfuric acid or hydrochloric acid can be used. When adding the neutralizing agent to the reaction solution, it may be added in the form of an aqueous solution in advance.

[0054] As the amount of the chain organic substance in the reaction solution increases, the particle size (average particle size) of the resulting copper powder also becomes finer. In other words, the average particle size of the copper powder can be controlled by the amount of the chain organic substance. Furthermore, the incorporation of the chain organic substance into the organic coating formed on the surface of the copper powder improves sinterability. The amount of the chain organic substance in the reaction solution is set according to conditions such as the particle size of the copper powder obtained after the reduction reaction. The amount of the chain organic substance in the reaction solution can be set through preliminary experiments. The amount of the chain organic substance in the reaction solution is preferably 10% by mass or less relative to the total amount of copper contained in the raw copper oxide. Furthermore, the amount of the chain organic substance in the reaction solution (the amount of the chain organic substance added to polyol solvent A) is preferably 0.005% by mass or more relative to the total amount of copper contained in the raw copper oxide. Furthermore, the amount of the chain organic substance in the reaction solution is preferably 0.005% by mass or more and 10% by mass or less relative to the total amount of copper contained in the raw copper oxide. Addition of the chain organic substance in an amount less than 0.005% by mass relative to the total amount of copper contained in the raw copper oxide may be insufficient to exert the effects of particle size control and sinterability improvement. Furthermore, since the effect of adding the chain organic substance gradually decreases as the amount added increases, addition of the chain organic substance in an amount exceeding 10% by mass relative to the total amount of copper contained in the raw copper oxide increases production costs and is therefore uneconomical. The amount of the chain organic substance in the reaction solution (the amount of the chain organic substance added to polyol solvent A) is preferably 0.001 mol % or more, and may be, for example, 0.01 mol % or more, or 0.1 mol % or more, relative to the total amount of copper contained in the raw copper oxide. The amount of the chain organic substance in the reaction solution is preferably 1 mol % or less, and may be, for example, 0.001 mol % or more and 1 mol % or less, relative to the total amount of copper contained in the raw copper oxide.

[0055] The average particle size of the copper powder obtained by the copper powder manufacturing method 1 according to this embodiment is preferably 250 nm or less. The copper powder (polyol copper powder) obtained by the manufacturing method described above can be controlled to be equal to or less than the above average particle size by using the chain organic substance during the reduction reaction. Because it is a fine copper powder, it can be used for electronic components such as electrodes of multilayer ceramic capacitors. For example, by using the copper powder manufacturing method 1, copper powders having average particle sizes of 200 nm or less, 150 nm or less, 110 nm or less, 100 nm or less, 90 nm or less, 70 nm or less, and 60 nm or less can be obtained, as described in the examples.

[0056] As described above, the copper powder manufacturing method 1 of this embodiment is a copper powder manufacturing method characterized by mixing copper oxide powder with a polyol solvent having a boiling point of 230°C or less to which the chain organic substance has been added, to obtain a copper oxide powder slurry, and heating the resulting mixture at 230°C or less. The copper powder manufacturing method 1 of this embodiment is a method capable of manufacturing the copper powder of this embodiment. Note that, in the copper powder manufacturing method 1 of this embodiment, configurations other than those described above are optional. According to the copper powder manufacturing method 1 of this embodiment, copper powder having an organic coating that prevents the formation of an oxide coating that can inhibit sintering and excellent low-temperature sinterability can be obtained. Note that, in the copper powder manufacturing method 1 of this embodiment, substances other than those described above may be added to the reaction solution within the scope of the present invention.

[0057] (Method for Producing Copper Powder 2) Another aspect of the present embodiment of the copper powder manufacturing method includes a heat treatment step in which copper powder having an average particle size of 250 nm or less and not satisfying at least one of the conditions (3) and (4) for the copper powder of the present embodiment described above is dispersed in a polyol solvent having a boiling point of 250°C or higher to which the chain organic compound has been added (hereinafter, the polyol solvent having a boiling point of 250°C or higher may be referred to as polyol solvent B) (hereinafter, the liquid in which the polyol solvent B and the copper powder are mixed and suspended may be collectively referred to as the "treatment liquid") and heated to obtain the target copper powder. The heat treatment step allows modification of the organic compound on the surface of the copper powder, including application of the chain organic compound to the copper powder surface. This allows the copper powder of the present embodiment to be obtained. For example, copper powder manufacturing method 2 can be used to obtain copper powders having an average particle size of 200 nm or less, 150 nm or less, 110 nm or less, 100 nm or less, 90 nm or less, 70 nm or less, or 60 nm or less, as described in the examples.

[0058] The copper powder having an average particle size of 250 nm or less and not satisfying at least one of the conditions (3) and (4) of the copper powder in this embodiment is, for example, copper powder produced by the copper powder production method described in JP 2022-128445 A. Of course, the copper powder is not limited thereto, and copper powder produced by other wet methods or vapor phase methods may also be used as long as it does not satisfy at least one of the conditions (3) and (4) of the copper powder in this embodiment.

[0059] The polyol solvent B used in the heat treatment step is a polyol having a boiling point of 250°C or higher, and is preferably one or more selected from the group consisting of triethylene glycol (boiling point: 287°C), tetraethylene glycol (boiling point: 327°C), and polyethylene glycol (boiling point: around 300°C) having an average molecular weight of 200 to 600. The amount of the chain organic substance added is preferably 10% by mass or less, based on the total amount of copper contained in the copper powder to be treated. The amount of the chain organic substance added is preferably 0.005% by mass or more, based on the total amount of copper contained in the copper powder to be treated. The amount of the chain organic substance added is preferably 0.005% by mass or more, based on the total amount of copper contained in the copper powder to be treated. The amount of the chain organic substance added is preferably 0.005% by mass or more, based on the total amount of copper contained in the copper powder to be treated.

[0060] The heat treatment temperature in the heat treatment step is preferably 230°C or higher. The heat treatment temperature can be set, for example, as conditions described in the Examples, and can be 240°C or higher, 250°C or higher, 260°C or higher, or 270°C or higher. The heat treatment temperature is preferably ±0°C or lower relative to the boiling point of polyol solvent B, and more preferably -5°C or lower relative to the boiling point of polyol solvent B. The heat treatment temperature is preferably 230°C or higher and ±0°C or lower relative to the boiling point of polyol solvent B, more preferably 250°C or higher and -5°C or lower relative to the boiling point of polyol solvent B, and even more preferably 270°C or higher and -5°C or lower relative to the boiling point of polyol solvent B. If the heat treatment temperature is lower than 230°C, the substitution of organic matter on the copper powder surface will not proceed sufficiently, and the desired organic coating will not be formed, making it impossible to impart excellent oxidation resistance and low-temperature sintering properties to the copper powder. Furthermore, if the heat treatment temperature is higher than the boiling point of polyol solvent B, the polyol solvent may be significantly reduced (consumed) due to decomposition and volatilization, which may result in insufficient heat treatment. The heat treatment time is preferably within 1 hour, more preferably within 30 minutes, and even more preferably within 15 minutes.

[0061] In the heat treatment step, copper powder that does not satisfy at least one of the conditions (3) and (4) for the copper powder of this embodiment is heated in polyol solvent B to which the chain organic substance has been added to obtain the copper powder of this embodiment. In the heat treatment step, heating is started after the chain organic substance has been added to the treatment liquid. However, the chain organic substance may also be added later to the reaction liquid while the temperature is being increased.

[0062] When using a chain organic substance that does not become neutral (pH of about 6.5 to 7.5) when made into an aqueous solution, it is preferable to add an alkali or acid as a neutralizing agent to neutralize the chain organic substance added to the treatment solution. When an alkali is used as the neutralizing agent, an alkali metal hydroxide is preferred, and specifically, sodium hydroxide or potassium hydroxide can be used. When an acid is used as the neutralizing agent, an inorganic acid is preferred, and specifically, sulfuric acid or hydrochloric acid can be used. When the neutralizing agent is added to the reaction solution, it may be prepared in advance as an aqueous solution and then added.

[0063] The chain organic substance in the treatment solution also functions as a copper powder anti-linking agent. The amount of the chain organic substance in the treatment solution is set depending on conditions such as the particle size of the copper powder to be treated. The amount of the chain organic substance in the treatment solution can be set through preliminary experiments. The amount of the chain organic substance in the treatment solution is preferably 10% by mass or less relative to the total amount of copper contained in the copper powder to be treated. Furthermore, the amount of the chain organic substance in the treatment solution (the amount of the chain organic substance added to polyol solvent B) is preferably 0.005% by mass or more relative to the total amount of copper contained in the copper powder to be treated. Furthermore, the amount of the chain organic substance in the treatment solution is preferably 0.005% by mass or more and 10% by mass or less relative to the total amount of copper contained in the copper powder to be treated. Addition of the chain organic substance in an amount less than 0.005% by mass relative to the total amount of copper contained in the copper powder to be treated is insufficient to exhibit the effect as a copper powder anti-linking agent. Furthermore, since the effect of adding the chain organic substance gradually decreases with increasing addition amount, adding the chain organic substance in an amount exceeding 10 mass% relative to the total amount of copper contained in the copper powder to be treated increases production costs and is therefore uneconomical. Furthermore, the amount of the chain organic substance in the treatment solution (the amount of the chain organic substance added to polyol solvent B) is preferably 0.001 mol% or more relative to the total amount of copper contained in the copper powder to be treated, and may be, for example, 0.01 mol% or more or 0.1 mol% or more. Furthermore, the amount of the chain organic substance in the treatment solution is preferably 1 mol% or less relative to the total amount of copper contained in the copper powder to be treated. Furthermore, the amount of the chain organic substance in the treatment solution is preferably 0.001 mol% or more but 1 mol or less relative to the total amount of copper contained in the copper powder to be treated, and may be 0.01 mol% or more but 1 mol or less.

[0064] As described above, the copper powder manufacturing method 2 of this embodiment is a copper powder manufacturing method characterized by mixing copper powder having an average particle size of 250 nm or less and not satisfying at least one of the conditions (3) and (4) described for the copper powder of this embodiment with a polyol solvent having a boiling point of 250°C or higher to which the chain organic substance has been added, to obtain a copper powder slurry, and then heat-treating the resulting mixture at 230°C or higher. The copper powder manufacturing method 2 of this embodiment is a method capable of producing the copper powder of this embodiment. Note that, in the copper powder manufacturing method 2 of this embodiment, the other components are optional. According to the copper powder manufacturing method 2 of this embodiment, copper powder having an organic coating that prevents the formation of an oxide coating that can inhibit sintering and excellent low-temperature sinterability can be obtained. Note that, in the copper powder manufacturing method 2 of this embodiment, substances other than those described above may be added to the reaction solution within the scope of the present invention.

[0065] The present invention will be explained in more detail below by showing examples and comparative examples, but the present invention is not limited to the following examples. In the following description, the polyol solvent used in the reduction step is referred to as the first polyol solvent, and the polyol solvent used in the heat treatment step is referred to as the second polyol solvent. The physical property values ​​were measured as follows.

[0066] (1) Average particle size The average particle size of the obtained copper powder (polyol copper powder) is the number-average particle size determined from image analysis of 200 or more particles observed with a scanning electron microscope (SEM). (2) Analysis of organic matter on the copper powder surface To determine the organic components on the copper powder surface, 10 mg of copper powder was immersed in 70 μl of a 1 wt % tetramethylammonium hydroxide-methanol solution to extract the organic matter from the surface, and the powder was dried at 50°C for 10 minutes. The organic components were then gasified in a pyrolysis furnace (PY-3030D manufactured by Frontier Labs) at 300°C for 30 seconds, and detected by GC / MS (GC part: GC-2010Plus, MS part: QP-2010Ultra manufactured by Shimadzu Corporation) in the m / z range of 33 to 550. <Gas chromatographic conditions> Column: UltraALLOY manufactured by Frontier Labs +-5 30m x inner diameter 0.25mm Carrier gas: Helium Temperature program: 50-350°C, 10°C / min Injection method: Split (split ratio 20:1) Injection port temperature: 300°C In parallel, 0.5g of copper powder was immersed in 10ml of 0.5N sodium hydroxide aqueous solution to extract organic matter from the surface, and the supernatant after centrifugation was used as an evaluation sample and detected by LC / MS (Agilent Technologies, LC part: Agilent 1290 infinity2, MS part: Agilent 6530). Qualitative analysis of the organic components was performed from the data obtained above. <Liquid chromatographic conditions> Column: Waters ACQUITY UPLC BEH C18 1.7 μm × 150 mm Column temperature: 40°C Flow rate: 0.2 ml / min Injection volume: 5 μl Eluent: Pure water / acetonitrile mixture: 0-22.5 minutes... 99.5 / 0.5, 22.51-30 minutes... 0 / 100, 30.01-35 minutes... 99.5 / 0.5 <Mass spectrometry conditions (for LC)> Polarity: Positive Measurement mass range: m / z = 70-1700 Ionization method: ESI Gas temperature, flow rate: 280°C, 12 L / min Nebulizer pressure: 55 psi Sheath gas temperature, flow rate: 350°C, 12 L / min Fragmenter: 100 V Scan rate: 3 spec / sec (3) Measurement of Thermal Shrinkage Behavior (TMA) The thermal shrinkage behavior of the obtained copper powder was measured using a thermomechanical analyzer (TMA) (TMA4000SA, manufactured by BRUKER Corporation). Approximately 0.3 g of copper powder was weighed and filled into a mold having a cylindrical hole with an inner diameter of 5 mm. A load of 100 MPa was applied in a press for 1 minute to form a green compact with a diameter of 5 mm and a height of 2 to 4 mm. The shrinkage rate in the thickness (height) direction of the green compact was measured when heated from 25°C under the following conditions, and the temperatures at which the thermal shrinkage rate became 1% and 3% based on the green compact thickness at 25°C were determined. Heating rate: 10°C / min. Temperature range: room temperature to 800°C. Applied load: 98 mN. Atmosphere: pure nitrogen (inert atmosphere) or 2% by volume of H 2 +98 capacity%-N 2 (reducing atmosphere)

[0067] (Example 1) [Reduction step] Cuprous oxide (Cu) was used as copper oxide powder. 2 3.6 g of O) powder (manufactured by Chemet, product number: Ultrafine) was placed in a 50 ml tall beaker, and 13.5 g of propylene glycol (abbreviation: PG, boiling point: 188°C, molecular weight: 76) was added as the first polyol solvent. Then, 0.302 g of poly(ethylene glycol) bis(carboxymethyl) ether (average molecular weight: 600) (abbreviation: PEG600 dibasic acid, manufactured by Sigma-Aldrich) (9.44% by mass (1 mol%) relative to the total amount of copper in the cuprous oxide) and 162 μl of a 25% by volume aqueous sodium hydroxide solution were added for neutralization and mixed to form a uniform slurry. This slurry was heated to 185°C and maintained at that temperature for 45 minutes while stirring, allowing the reduction reaction to occur. After cooling the reaction solution, the resulting polyol copper powder was centrifuged, washed, and dried.

[0068] Example 2 Polyol copper powder was obtained in the same manner as in Example 1, except that the first polyol solvent was changed to 1,3-propanediol (abbreviation: 1,3-PDO, boiling point: 214° C., molecular weight: 76).

[0069] Example 3 Polyol copper powder was obtained in the same manner as in Example 1, except that the first polyol solvent was changed to 1,2-butanediol (abbreviation: 1,2-BDO, boiling point: 194° C., molecular weight: 90).

[0070] Example 4 Polyol copper powder was obtained in the same manner as in Example 1, except that the first polyol solvent was changed to 1,3-butanediol (abbreviation: 1,3-BDO, boiling point: 207° C., molecular weight: 90).

[0071] Example 5 A polyol copper powder was obtained in the same manner as in Example 3, except that the amount of PEG 600 dibasic acid added was 0.0302 g (0.94 mass % (0.1 mol %) relative to the total amount of copper in the cuprous oxide) and 16 μl of a 25 mass vol % aqueous sodium hydroxide solution was added for neutralization.

[0072] Example 6 A polyol copper powder was obtained in the same manner as in Example 3, except that the amount of PEG 600 dibasic acid added was 0.0030 g (0.094 mass % (0.01 mol %) relative to the total amount of copper in the cuprous oxide) and 16 μl of a 25 mass vol % aqueous sodium hydroxide solution was added for neutralization.

[0073] Example 7 A polyol copper powder was obtained in the same manner as in Example 3, except that the amount of PEG 600 dibasic acid added was 0.0003 g (0.0094 mass % (0.001 mol %) relative to the total amount of copper in the cuprous oxide) and 16 μl of a 25 mass vol % aqueous sodium hydroxide solution was added for neutralization.

[0074] Example 8 [Reduction Step] Copper powder was prepared by the method of Example 5 described in JP 2022-128445 A. Specifically, 27 g of cuprous oxide powder (copper oxide powder) was placed in a 200 ml separable flask, and 100 g of ethylene glycol (abbreviated as EG, boiling point: 197°C, molecular weight: 62) was added as a first polyol solvent. Then, 0.65 g of cis-1,2-cyclohexanedicarboxylic acid (2.71% by mass (1 mol%) relative to the total amount of copper in the cuprous oxide) and 1.21 ml of a 25% by volume aqueous sodium hydroxide solution for neutralization were added and mixed to form a uniform slurry. This slurry was heated to 190°C and maintained at that temperature for 45 minutes while stirring, allowing the reduction reaction to occur. After cooling the reaction solution, the resulting polyol copper powder was centrifuged, washed, and dried. [Heat Treatment Step] 3.2 g of copper powder was collected from the resulting centrifuged polyol copper powder and redispersed in 13.5 g of tetraethylene glycol (TeEG, boiling point: 327°C, molecular weight: 194) as a second polyol solvent. Subsequently, 0.302 g of poly(ethylene glycol) bis(carboxymethyl) ether (average molecular weight 600) (PEG600 dibasic acid) (9.44% by mass (1 mol%) relative to the total amount of copper in the treated copper) and 162 μl of 25% by volume aqueous sodium hydroxide solution for neutralization were added and mixed to form a uniform slurry. This slurry was heated to 280°C and maintained at that temperature for 10 minutes while stirring, performing a heat treatment. After cooling the reaction solution, the resulting heat-treated polyol copper powder was centrifuged, washed, and dried.

[0075] Example 9 The same procedure as in Example 8 was carried out except that the temperature of the reduction reaction was changed to 180° C., to obtain a heat-treated polyol copper powder.

[0076] Example 10 [Reduction Step] Copper powder was prepared by the method of Example 24 described in JP 2022-128445 A. Specifically, 27 g of cuprous oxide powder (copper oxide powder) was placed in a 200 ml separable flask, and 100 g of propylene glycol (abbreviation: PG, boiling point: 188°C, molecular weight: 76) was added as a first polyol solvent. Then, 0.65 g of cis-1,2-cyclohexanedicarboxylic acid (2.71% by mass (1 mol%) relative to the total amount of copper in the cuprous oxide) and 1.21 ml of a 25% by volume aqueous sodium hydroxide solution for neutralization were added and mixed to form a uniform slurry. This slurry was heated to 185°C and maintained at that temperature for 45 minutes while stirring, allowing the reduction reaction to occur. After cooling the reaction solution, the resulting polyol copper powder was centrifuged, washed, and dried. [Heat Treatment Step] 3.2 g of copper powder was separated from the resulting polyol copper powder after centrifugation and redispersed in 13.5 g of tetraethylene glycol as a second polyol solvent. Subsequently, 0.302 g of poly(ethylene glycol) bis(carboxymethyl) ether (average molecular weight 600) (PEG600 dibasic acid) (9.44 mass% (1 mol%) relative to the total amount of copper in the treated copper) and 162 μl of 25% by volume aqueous sodium hydroxide solution for neutralization were added and mixed to form a uniform slurry. This slurry was heated to 280°C and maintained at that temperature for 10 minutes while stirring, thereby performing a heat treatment. After cooling the reaction solution, the resulting heat-treated polyol copper powder was centrifuged, washed, and dried.

[0077] Example 11 A polyol copper powder was obtained in the same manner as in Example 10, except that in the heat treatment step, the amount of PEG 600 dibasic acid added was 0.0302 g (0.94 mass % (0.1 mol %) relative to the total amount of copper in the treated copper) and 16 μl of a 25 mass vol % aqueous sodium hydroxide solution was added for neutralization.

[0078] Example 12 A polyol copper powder was obtained in the same manner as in Example 10, except that in the heat treatment step, the amount of PEG 600 dibasic acid added was 0.0030 g (0.094 mass % (0.01 mol %) relative to the total amount of copper in the treated copper) and 16 μl of a 25 mass vol % aqueous sodium hydroxide solution was added for neutralization.

[0079] Example 13 A polyol copper powder was obtained by the same procedure as in Example 10, except that in the heat treatment step, the amount of PEG 600 dibasic acid added was 0.0003 g (0.0094 mass % (0.001 mol %) relative to the total amount of copper in the treated copper) and 16 μl of a 25 mass vol % aqueous sodium hydroxide solution was added for neutralization.

[0080] Example 14 The same procedure as in Example 10 was carried out except that the heating temperature of the slurry in the heat treatment step was 260° C., to obtain a heat-treated polyol copper powder.

[0081] Example 15 The same procedure as in Example 10 was carried out except that the heating temperature of the slurry in the heat treatment step was 240° C., to obtain a heat-treated polyol copper powder.

[0082] Example 16 The same procedure as in Example 10 was carried out except that the heating temperature of the slurry in the heat treatment step was 230° C., to obtain a heat-treated polyol copper powder.

[0083] Example 17 A heat-treated polyol copper powder was obtained in the same manner as in Example 10, except that 0.1724 g (5.39 mass % (1 mol %) of eicosanedioic acid with respect to the total amount of copper in the treated copper) was added instead of poly(ethylene glycol) bis(carboxymethyl) ether (average molecular weight 600) (PEG600 dibasic acid) in the heat treatment step.

[0084] Example 18 A heat-treated polyol copper powder was obtained in the same manner as in Example 10, except that 0.1018 g of sebacic acid (3.18 mass % (1 mol %) based on the total amount of copper in the treated copper) was added instead of poly(ethylene glycol) bis(carboxymethyl) ether (average molecular weight 600) (PEG600 dibasic acid) in the heat treatment step.

[0085] Example 19 A heat-treated polyol copper powder was obtained in the same manner as in Example 10, except that 0.1159 g (3.63 mass % (1 mol %) based on the total amount of copper in the treated copper) of dodecanedioic acid was added instead of poly(ethylene glycol) bis(carboxymethyl) ether (average molecular weight 600) (PEG600 dibasic acid) in the heat treatment step.

[0086] Comparative Example 1 [Reduction Step] 30 g of copper oxide (CuO) powder (Furukawa Chemicals, product number: FCO-M6) was placed in a 200 ml separable flask as copper oxide powder, and 100 g of tetraethylene glycol was added as a first polyol solvent, followed by mixing to form a uniform slurry. This slurry was heated to 300°C and maintained at that temperature for 45 minutes while stirring, allowing the reduction reaction to occur. After cooling the reaction solution, the resulting polyol copper powder was centrifuged, washed, and dried.

[0087] Comparative Example 2 Polyol copper powder was obtained in the same manner as in Example 2, except that PEG 600 dibasic acid and the 25% by volume aqueous solution of sodium hydroxide for neutralization were not added in the reduction step.

[0088] Comparative Example 3 Polyol copper powder was obtained in the same manner as in Example 3, except that PEG 600 dibasic acid and the 25% by volume aqueous solution of sodium hydroxide for neutralization were not added in the reduction step.

[0089] Comparative Example 4 Polyol copper powder was obtained in the same manner as in Example 4, except that PEG 600 dibasic acid and the 25% by volume aqueous solution of sodium hydroxide for neutralization were not added in the reduction step.

[0090] Conventional Example 1 [Reduction Step] Copper powder was produced by the method of Example 5 described in JP 2022-128445 A. After cooling the reaction solution, the produced polyol copper powder was centrifuged, washed, and dried. Unlike Example 8, this polyol copper powder was not subjected to a heat treatment.

[0091] Conventional Example 2 Polyol copper powder was obtained in the same manner as in Conventional Example 1, except that the temperature of the reduction reaction was changed to 180° C. Unlike Example 9, this polyol copper powder was not subjected to a heat treatment.

[0092] Conventional Example 3 [Reduction Step] Copper powder was produced by the method of Example 24 described in JP 2022-128445 A. After cooling the reaction solution, the produced polyol copper powder was centrifuged, washed, and dried. Unlike Examples 10 to 19, this polyol copper powder was not subjected to a heat treatment.

[0093] Comparative Example 5 The same procedure as in Example 10 was carried out except that the heating temperature of the slurry in the heat treatment step was 200° C., to obtain a heat-treated polyol copper powder.

[0094] Comparative Example 6 A polyol copper powder was obtained in the same manner as in Example 10, except that PEG 600 dibasic acid and the 25% by volume aqueous solution of sodium hydroxide were not added in the heat treatment step.

[0095] The manufacturing conditions for Examples 1 to 19, Comparative Examples 1 to 6, and Conventional Examples 1 to 3 are shown in Table 1.

[0096] (Evaluation Results) For the polyol copper powders obtained in Examples 1 to 19, Comparative Examples 1 to 6, and Conventional Examples 1 to 3, the average particle size was measured using the methods described above. Surface organic matter on the copper powder was detected by GC / MS and LC / MS. TMA measurements were also performed to determine the temperature at which the thermal shrinkage of a compact of the polyol copper powder obtained in an inert atmosphere reached 1% (hereinafter sometimes abbreviated as TMA 1%), and the temperature difference (absolute value) between the temperature at which the thermal shrinkage of the compact in an inert atmosphere reached 3% (hereinafter sometimes abbreviated as TMA 3%) and the temperature at which the thermal shrinkage of the compact in a reducing atmosphere reached 3%. These results are shown in Table 2. In Table 2, "not detected" means that the value was below the detection limit. The GC / MS results for Example 17 and Conventional Example 3 are shown in Figure 2.

[0097]

[0098] In all Examples, organic substances satisfying the aforementioned conditions (1) and (2) were detected by GC / MS and LC / MS. Furthermore, the temperature at which 1% TMA was reached in an inert atmosphere was 230°C or lower in all Examples, and the temperature difference between the temperatures at which 3% TMA was reached in an inert atmosphere and a reducing atmosphere was less than 10°C. For example, as shown in the temperature-TMA profile of Example 10 ( FIG. 1 ), there is almost no change in the sintering (thermal shrinkage) behavior in an inert atmosphere and a reducing atmosphere, and it can be seen that no oxide film that inhibits sintering is formed on the surface of the copper powder, or that the oxide film is thin enough not to inhibit sintering.

[0099] On the other hand, in both the Comparative Example and the Conventional Example, no organic substance satisfying both the above-mentioned conditions (1) and (2) was detected by GC / MS and LC / MS. Furthermore, the temperature at which 1% TMA was reached in an inert atmosphere exceeded 230°C in Conventional Examples 1 to 3, and the temperature difference at which 3% TMA was reached in an inert atmosphere and in a reducing atmosphere was 10°C or more in both the Comparative Example and the Conventional Example.

[0100] In Comparative Example 1, although the copper powder surface was coated with an organic substance that could be detected by GC / MS and satisfied the aforementioned condition (1), no organic substance that could be detected by LC / MS and satisfied the aforementioned condition (2) was present on the copper powder surface. Therefore, compared with Examples 1 to 4, the surface coating with organic substance was insufficient, and an oxide film that inhibits sintering was likely to form on the copper powder surface. This is thought to have resulted in a deterioration in sinterability in an inert atmosphere, resulting in a difference in sintering behavior from that in a reducing atmosphere (the aforementioned condition (4) was not satisfied).

[0101] In Comparative Examples 2 to 5 and Conventional Examples 1 to 3, the organic matter detected by GC / MS was not one that satisfied the aforementioned condition (1), and therefore it is believed that the organic matter on the copper powder surface inhibited sintering, thereby failing to satisfy the aforementioned condition (3). Furthermore, because no organic matter detectable by LC / MS that satisfied the aforementioned condition (2) was present on the copper powder surface, an oxide film that inhibits sintering was likely to form on the copper powder surface, which deteriorated the sinterability under an inert atmosphere and resulted in a difference in sintering behavior compared to under a reducing atmosphere. (The aforementioned condition (4) was not satisfied.)

[0102] In Comparative Example 6, the copper powder particles aggregated during the heat treatment to form large lumps, making subsequent analysis impossible. This is thought to be because a chain organic substance that functions as an inhibitor for preventing copper powder linkage was not added.

[0103] Since Examples 8 to 19 were obtained by heat-treating Conventional Examples 1 to 3, respectively, it is believed that the heat treatment reconstructed organic substances on the surface of the copper powder that satisfied the aforementioned conditions (1) and (2) by GC / MS and LC / MS, resulting in copper powders that satisfied the aforementioned conditions (3) and (4).

[0104] From the examples, comparative examples, and conventional examples, it is confirmed that the copper powder in this embodiment has an average particle size of 250 nm or less, and is surface-coated with both a specific organic substance detected by GC / MS and a specific organic substance detected by LC / MS; when a green compact obtained by pressure-molding the copper powder at 100 MPa is heated in an inert atmosphere from 25°C at a temperature increase rate of 10°C / min, the temperature at which the green compact reaches a thermal shrinkage of 1% is 230°C or less, and when a green compact obtained by pressure-molding the copper powder at 100 MPa is heated in an inert atmosphere and a reducing atmosphere from 25°C at a temperature increase rate of 10°C / min, the temperature difference between the temperature at which the green compact reaches a thermal shrinkage of 3% in the inert atmosphere and the temperature at which the green compact reaches a thermal shrinkage of 3% in the reducing atmosphere is less than 10°C,

[0105] The technical scope of the present invention is not limited to the aspects described in the above-mentioned embodiments. One or more of the requirements described in the above-mentioned embodiments may be omitted. The requirements described in the above-mentioned embodiments may be combined as appropriate. Furthermore, to the extent permitted by law, the disclosures of Japanese Patent Application No. 2022-030202 and all documents cited in the above-mentioned embodiments are incorporated by reference into the present description.

[0106] The present invention includes the following embodiments. [1] Copper powder having an average particle size of 250 nm or less and a surface coated with an organic substance, which satisfies all of the following conditions (1) to (4): Condition (1) When the organic substance present on the surface of the copper powder is detected by gas chromatography mass spectrometry, the organic substance is found to be H(—O—CH 2 -CH 2 ) n -OH (where n is an integer of 1 or more and 4 or less), HOOC-CH 2 (-O-CH 2 -CH 2 ) m -OH (where m is an integer of 1 or more and 3 or less), HOOC-CH 2 (-O-CH 2 -CH 2 ) l -O-CH 2 -COOH (where l is 1 or 2), H(-C 3 H 6 O) s -OH (where s is an integer of 1 or more and 4 or less), HOOC-CH(CH 3 ) (-C 3 H 6 O) t -OH (where t is an integer of 1 or more and 3 or less), HOOC-CH(CH 3 ) (-C 3 H 6 O) u -O-CH(CH 3)-COOH (where u is 1 or 2). Condition (2) When the organic matter present on the surface of the copper powder is detected by liquid chromatography mass spectrometry, it is found to be a chain organic matter with a molecular weight of 200 to 1000, and the chain organic matter has at each end of the molecule a carboxy group (-COOH), a hydroxy group (-OH), an amino group (-NH 2 ), aldehyde group (-CHO), nitro group (-NO 2 ), thiol group (-SH), sulfo group (-SO 3 HHH), phosphate group (-PO 4 H 2), a chain organic substance having one selected from the group consisting of a cyan group (-CN), a chloro group (-Cl), a bromo group (-Br), and an iodine group (-I) is detected. Condition (3) When a green compact obtained by compacting the copper powder is heated from 25°C under an inert atmosphere, the temperature at which the thermal shrinkage is 1% is 230°C or less, in a measurement of the thermal shrinkage based on the thickness of the green compact at 25°C. Condition (4) When a green compact obtained by compacting the copper powder is heated from 25°C under an inert atmosphere and a reducing atmosphere, the temperature difference between the temperature at which the thermal shrinkage is 3% under the inert atmosphere and the temperature at which the thermal shrinkage is 3% under the reducing atmosphere is less than 10°C, in a measurement of the thermal shrinkage based on the thickness of the green compact at 25°C. [2] The copper powder according to [1], characterized in that the average particle size is 200 nm or less. [3] The copper powder according to [1] or [2], characterized in that the average particle size is 150 nm or less. [4] A method for producing copper powder according to any one of [1] to [3], comprising mixing copper oxide powder with a polyol solvent having a boiling point of 230° C. or less to which the chain organic substance has been added, to obtain a copper oxide powder slurry, and heating the resulting slurry at 230° C. or less. [5] A method for producing copper powder according to [4], characterized in that the amount of the chain organic substance added is 0.005 mass % or more and 10 mass % or less relative to the total amount of copper contained in the copper oxide powder. [6] The method for producing copper powder according to [4] or [5], wherein the polyol solvent having a boiling point of 230°C or less is one or more selected from the group consisting of ethylene glycol (boiling point: 196°C), propylene glycol (boiling point: 188°C), 1,3-propanediol (boiling point: 214°C), 1,2-butanediol (boiling point: 194°C), 1,3-butanediol (boiling point: 207°C), 1,4-butanediol (boiling point: 228°C), 1,2-pentanediol (boiling point: 210°C), and 1,2-hexanediol (boiling point: 223°C).[7] The method for producing copper powder according to any one of [1] to [3], characterized in that copper powder having an average particle size of 250 nm or less and not satisfying at least one of the conditions (3) and (4) described in [1] is mixed with a polyol solvent having a boiling point of 250°C or higher to which the chain organic substance has been added, to obtain a copper powder slurry, and then heat-treating the resulting mixture at 230°C or higher. [8] The method for producing copper powder according to [7], characterized in that the amount of the chain organic substance added is 0.005% by mass to 10% by mass, based on the total amount of copper contained in the copper powder to be heat-treated. [9] The method for producing copper powder according to [7] or [8], characterized in that the polyol solvent having a boiling point of 250°C or higher is one or more selected from the group consisting of triethylene glycol (boiling point: 287°C), tetraethylene glycol (boiling point: 327°C), and polyethylene glycol (boiling point: around 300°C) having an average molecular weight of 200 to 600.

[10] The method for producing copper powder according to any one of [7] to [9], characterized in that the temperature of the heat treatment is 250° C. or higher.

[11] The method for producing copper powder according to any one of [7] to

[10] , characterized in that the temperature of the heat treatment is 270° C. or higher.

Claims

1. The copper powder has an average particle size of 250 nm or less and a surface coated with an organic substance, and satisfies all of the following conditions (1) to (4): (1) When organic matter present on the surface of the copper powder is detected by gas chromatography mass spectrometry, H(-O-CH 2 -CH 2 ) n -OH (where n is an integer of 1 or more and 4 or less), HOOC-CH 2 (-O-CH 2 -CH 2 ) m -OH (where m is an integer of 1 or more and 3 or less), HOOC-CH 2 (-O-CH 2 -CH 2 ) l -O-CH 2 -COOH (where l is 1 or 2), H(-C 3 H 6 O) s -OH (where s is an integer of 1 or more and 4 or less), HOOC-CH(CH 3 ) (-C 3 H 6 O) t -OH (where t is an integer of 1 or more and 3 or less), HOOC-CH(CH 3 ) (-C 3 H 6 O) u -O-CH(CH 3 )--COOH (wherein u is 1 or 2), (2) When organic matter present on the surface of the copper powder is detected by liquid chromatography mass spectrometry, The chain organic substance has a molecular weight of 200 to 1000, and the chain organic substance has a carboxy group (-COOH), a hydroxy group (-OH), an amino group (-NH 2 ), aldehyde group (-CHO), nitro group (-NO 2 ), thiol group (-SH), sulfo group (-SO 3 H), phosphate group (-PO 4 H 2 A chain organic substance having one selected from the group consisting of a cyan group (-CN), a chloro group (-Cl), a bromo group (-Br), and an iodine group (-I) is detected. (3) When a green compact obtained by pressing the copper powder is heated from 25° C. in an inert atmosphere, the temperature at which the thermal shrinkage becomes 1% is 230° C. or lower, in measurement of the thermal shrinkage based on the thickness of the green compact at 25° C. (4) When a green compact obtained by pressing the copper powder is heated from 25° C. under an inert atmosphere and under a reducing atmosphere, the temperature difference between the temperature at which the heat shrinkage rate is 3% under an inert atmosphere and the temperature at which the heat shrinkage rate is 3% under a reducing atmosphere is less than 10° C. in measurement of the heat shrinkage rate based on the thickness of the green compact at 25° C.

2. 2. The copper powder according to claim 1, wherein the average particle size is 200 nm or less.

3. 2. The copper powder according to claim 1, wherein the average particle size is 150 nm or less.

4. The method for producing copper powder according to any one of claims 1 to 3, heating a copper oxide powder slurry obtained by mixing a copper oxide powder with a polyol solvent having a boiling point of 230° C. or less to which the chain organic substance has been added at a temperature of 230° C. or less; A method for producing copper powder comprising the steps of:

5. The amount of the chain organic substance added is 0.005% by mass or more and 10% by mass or less with respect to the total amount of copper contained in the copper oxide powder. The method for producing copper powder according to claim 4 .

6. The polyol solvent having a boiling point of 230° C. or less is at least one selected from the group consisting of ethylene glycol (boiling point: 196° C.), propylene glycol (boiling point: 188° C.), 1,3-propanediol (boiling point: 214° C.), 1,2-butanediol (boiling point: 194° C.), 1,3-butanediol (boiling point: 207° C.), 1,4-butanediol (boiling point: 228° C.), 1,2-pentanediol (boiling point: 210° C.), and 1,2-hexanediol (boiling point: 223° C.). The method for producing copper powder according to claim 4 .

7. The method for producing copper powder according to any one of claims 1 to 3, Copper powder having an average particle size of 250 nm or less and not satisfying at least one of the conditions (3) and (4) of claim 1 is mixed with a polyol solvent having a boiling point of 250° C. or more to which the chain organic substance has been added, and the resulting copper powder slurry is heat-treated at 230° C. or more. A method for producing copper powder comprising the steps of:

8. The amount of the chain organic substance added is 0.005% by mass or more and 10% by mass or less based on the total amount of copper contained in the copper powder to be heat-treated. The method for producing copper powder according to claim 7 .

9. The polyol solvent having a boiling point of 250° C. or more is at least one selected from the group consisting of triethylene glycol (boiling point: 287° C.), tetraethylene glycol (boiling point: 327° C.), and polyethylene glycol having an average molecular weight of 200 to 600 (boiling point: around 300° C.). The method for producing copper powder according to claim 7 .

10. The method for producing copper powder according to claim 7, characterized in that the temperature of the heat treatment is 250°C or higher.

11. The method for producing copper powder according to claim 7, characterized in that the temperature of the heat treatment is 270°C or higher.