Flame-retardant hook-and-loop fastener
Patent Information
- Application Number
- JP2024506306
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Priority Date
- 2023-03-06
- Filing Date
- 2023-03-06
- Publication Date
- 2024-11-14
AI Technical Summary
Conventional flame-retardant hook-and-loop fasteners face issues with flame retardancy retention due to peeling off of surface-applied flame retardants, loss of flexibility from back coat resins, and vertical undulations during manufacturing, which affect engagement force and appearance.
A woven flame-retardant hook-and-loop fastener using PPS multifilament yarns and heat-fusible core-sheath filaments, where the engaging elements are heat-shrunk to secure them to the base fabric without a back coat resin, ensuring no vertical undulations and maintaining flame retardancy.
The solution provides a flame-retardant hook-and-loop fastener with enhanced pull-out resistance, consistent engagement force, and improved appearance by eliminating vertical undulations and maintaining flexibility, suitable for high-temperature applications.
Abstract
Description
Flame-retardant hook-and-loop fastener
[0001] The present invention relates to a woven fabric-based flame-retardant hook-and-loop fastener that has excellent flame retardancy, in which engaging elements are unlikely to be pulled out of the woven fabric base even after repeated engagement and release, in which the hook-and-loop fastener hardly produces vertical undulations, has excellent engaging force, and can be made wide, and to a method for producing the same.
[0002] Conventionally, as a hook-and-loop fastener having a woven base fabric, a combination of a so-called woven hook fastener, which has a large number of hook-shaped engaging elements made of monofilament yarn on the surface of the same base fabric, and a so-called woven loop fastener, which has a large number of loop-shaped engaging elements made of multifilament yarn on the surface of the woven base fabric that can engage with the hook-shaped engaging elements, has been widely used in fields such as clothing, daily necessities, and industrial materials, because there is little damage to the engaging elements and little decrease in engaging force even when engaging and peeling is repeated.
[0003] In addition, so-called hook-and-loop coexisting woven surface fasteners, in which both the above-mentioned hook-shaped engaging elements and loop-shaped engaging elements are present in large numbers on the same surface of a woven base fabric, are also widely used because they can combine the functions of both hook and loop surface fasteners in a single type of surface fastener, eliminating the need to use both hook and loop surface fasteners in combination as with conventional surface fasteners.
[0004] In recent years, hook-and-loop fasteners have been widely used as a means for fastening parts, structural materials, and insulating materials, such as interior walls, ceiling materials, and flooring materials, in vehicles such as automobiles, trains, ships, and aircraft. High levels of flame retardancy are required for all of these applications, and the hook-and-loop fasteners used are also required to have high levels of flame retardancy. Furthermore, hook-and-loop fasteners with high levels of flame retardancy are also required in the fields of special clothing, such as work clothes for use in high-temperature environments such as blast furnaces and foundries, and firefighting uniforms, as well as in fields requiring flame retardancy and heat resistance, such as filter fasteners for high-temperature gases.
[0005] Various flame-retardant hook-and-loop fasteners have been proposed to meet these requirements. For example, a typical hook-and-loop fastener is one in which the surface of a normal fabric-based hook-and-loop fastener is impregnated with or coated with a resin containing a flame retardant to impart flame retardancy. However, such hook-and-loop fasteners have the problem that the flame retardant applied to the surface peels off with repeated engagement and release, or the flame retardant is lost by washing, etc., and the flame retardant effect cannot be sustained.
[0006] In addition, in the case of ordinary fabric-based hook-and-loop fasteners, a polyurethane or polyacrylic adhesive liquid called a back coat resin is applied to the back surface of the hook-and-loop fastener to prevent the engaging elements from being pulled out from the surface of the base fabric due to repeated engagement and release. However, when an adhesive is applied to the back surface, the hook-and-loop fastener loses its flexibility and becomes rigid, significantly degrading the texture of the fabric to which the hook-and-loop fastener is attached, and the increased rigidity makes it difficult to engage, and also reduces the engagement performance.
[0007] Furthermore, since the process speeds for weaving the hook-and-loop fastener and the process for applying a backcoat resin liquid to the back surface and drying it are significantly different, it becomes necessary to wind up the hook-and-loop fastener once in the middle, which makes the manufacture of the hook-and-loop fastener time-consuming and labor-intensive.Furthermore, in order to make the hook-and-loop fastener flame-retardant, it is necessary to add a flame retardant to the backcoat adhesive, but using such a backcoat adhesive containing a flame retardant causes problems such as the stability of the adhesive liquid and bleeding out of the flame retardant, and also causes problems such as a decrease in the backcoat effect.
[0008] As a technique for solving the problems of techniques for making hook-and-loop fasteners flame-retardant by impregnating and applying such flame retardant-added backcoat resin liquids, a flame-retardant woven hook-and-loop fastener has been proposed, in which threads constituting the hook-and-loop fastener are made of flame-retardant fibers, typically polyphenylene sulfide (hereinafter abbreviated as PPS) fibers, and a heat-fusible thread is used as part of the weft threads. For example, Patent Document 1 describes a method of weaving a hook-and-loop fastener fabric using PPS multifilament yarn as the warp yarn, a drawn yarn of multifilament yarn consisting of PPS multifilament yarn and heat-fusible core-sheath filament as the weft yarn, and PPS multifilament yarn or monofilament yarn as the engaging element yarn, the fabric being made of these warp yarns, weft yarn and engaging element yarn, with the engaging element yarn protruding in a loop shape on the surface, the heat-fusible component of the multifilament yarn consisting of the heat-fusible core-sheath filament being heat-melted to fuse and fix the yarns that make up the woven fabric base, and when the engaging element loop is made of monofilament yarn, cutting one leg of the loop to form a hook-shaped engaging element, thereby obtaining a flame-retardant hook-and-loop fastener.
[0009] In the case of a flame-retardant hook-and-loop fastener obtained based on the technology described in Patent Document 1, in order to achieve a high level of flame retardancy that can be used in fields that require an extremely high level of flame retardancy, such as automobiles and aircraft, it is effective to increase the proportion of PPS yarn that constitutes the hook-and-loop fastener and decrease the proportion of multifilament yarn made of heat-fusible sheath-core filaments. However, simply increasing the proportion of PPS yarn and decreasing the proportion of multifilament yarn made of heat-fusible sheath-core filaments results in insufficient fixation of the engaging elements by the heat-fusible components, and as a result, repeated engagement and release gradually releases the fixation of the engaging elements by the multifilament yarn made of heat-fusible sheath-core filaments, causing the engaging elements to be pulled out of the base fabric and resulting in a problem of a decrease in engaging force.
[0010] As an improved technology for a flame-retardant hook-and-loop fastener using such PPS yarn and a multifilament yarn made of a heat-fusible sheath-core filament, Patent Document 2 describes a technology in which a multifilament yarn made of a bundle of many thin PPS filaments is used as the PPS yarn used as part of the weft yarn, and a yarn having high heat shrinkability is used as the multifilament yarn made of a heat-fusible sheath-core filament used in combination with the multifilament yarn. With this technology, the multifilament yarn made of the heat-fusible sheath-core filament is highly heat-shrunk when heat-fused, tightening the base of the engaging elements, and the many thin PPS filaments can be wrapped around the engaging element yarn, making it possible to some extent to prevent the engaging elements from being pulled out of the base fabric due to repeated engagement and release, but a satisfactory level has not yet been reached.
[0011] Furthermore, when the technology of Patent Document 2 is used, large thermal shrinkage occurs when the multifilament yarn made of heat-fusible core-sheath filaments is thermally melted, causing the hook-and-loop fastener base fabric to ripple in the vertical direction (i.e., the hook-and-loop fastener rises and falls in the vertical direction like a piece of seaweed). The ripples occur in both the length direction (warp direction) and width direction (weft direction) of the hook-and-loop fastener, but since a highly shrinkable yarn is used for the weft, the ripples in the width direction are particularly large, which results in a major obstacle to the production of wide hook-and-loop fasteners.
[0012] In particular, for woven hook-and-loop fasteners, a method is generally adopted that provides excellent productivity, in which engaging element regions with engaging element loops and selvage regions without engaging element loops are each continuously present in the warp direction, and engaging element regions and selvage regions are alternately arranged in the weft direction, with a wide hook-and-loop fastener having multiple engaging element regions, and finally the centers of the selvage regions are slit parallel to the warp direction to simultaneously produce multiple hook-and-loop fasteners.For this reason, if the wide hook-and-loop fastener before slitting is wavy in the vertical direction, it is difficult to accurately slit the middle portions of the selvages, and the selvage width becomes narrower or wider, and furthermore, warp threads may fray from the slit selvage ends, resulting in inferior quality and appearance.
[0013] Furthermore, due to the occurrence of vertical undulations in the hook-and-loop fastener, when one leg of the loop for the hook-shaped engaging element is cut to form the hook-shaped engaging element, variations occur in the cut height of the loop, resulting in variations in the engaging force, or in some cases both legs are cut, some are only partially cut, or some are not cut and remain in a loop shape.
[0014] Furthermore, if the hook-and-loop fastener has ears with no engaging elements at both ends along the warp direction, and if the hook-and-loop fastener has vertical undulations, these ears also tend to wobble in the weft direction. When the hook-and-loop fastener is attached by sewing, these ears are sewn with a sewing thread, but if the ears wobble in the weft direction, the sewing thread appears to be meandering, which is a major problem in terms of appearance.
[0015] Furthermore, Patent Document 3 describes a method for coloring the flame-retardant PPS thread-based hook-and-loop fastener described in Patent Document 1, in which the flame-retardant PPS thread-based hook-and-loop fastener manufactured in Patent Document 1 is immersed in a bath containing a crosslinking agent and an aqueous dispersion in which a pigment is dispersed with a polymeric dispersant having ionic groups, and then removed from the bath. The fastener is then wrapped around a heated roll, dried, and heat-treated at 160°C for 10 minutes, and this process is repeated twice to cause a reaction between the ionic groups and the crosslinking agent, thereby firmly adhering the pigment to the surface of the hook-and-loop fastener. However, this method requires the hook-and-loop fastener to be loosely wrapped in order to prevent the engaging elements of the hook-and-loop fastener from collapsing during the heat treatment and to prevent the overlapping engaging element surfaces and back surfaces of the rolled hook-and-loop fastener from coming into close contact with each other and undergoing a crosslinking reaction, resulting in a strong bond between the two surfaces. Furthermore, simply wrapping the hook-and-loop fastener and heating it in this state does little to improve the waviness of the hook-and-loop fastener. Ultimately, the method described in this patent document does not improve the problems with the hook-and-loop fastener described above.
[0016] International Publication No. 2008 / 059958 Japanese Patent Application Laid-Open No. 2019-154880 Japanese Patent Application Laid-Open No. 2015-62599
[0017] The present invention provides a hook-and-loop fastener made of a flame-retardant PPS-based woven fabric that solves the above-mentioned problems, specifically, a hook-and-loop fastener that has excellent flame retardancy, in which the engaging elements are unlikely to be pulled out of the base fabric even after repeated engagement and release, has almost no vertical undulation, can be made wide, and can weave a wide hook-and-loop fastener in which the engaging element areas are divided in the weft direction by selvage areas, and can simultaneously obtain multiple hook-and-loop fasteners by slitting the selvage areas, and has no variation in the cut height of one leg of the hook-shaped engaging elements. The present invention also provides a flame-retardant woven hook-and-loop fastener with selvage that does not wobble in the weft direction.
[0018] That is, the present invention is a hook-and-loop fastener having a base fabric woven from warp yarns composed of PPS-based multifilament yarns, weft yarns composed of paralleled yarns of PPS-based multifilament yarns and multifilament yarns composed of heat-fusible filaments, and engaging element yarns composed of at least one type selected from the group consisting of PPS-based multifilament yarns and monofilament yarns, and engaging elements formed from the engaging element yarns present on the surface of the base fabric, wherein the warp yarns floating above and below the weft yarns sandwiched between them have a warp thickness in the base fabric thickness direction at the point where they are most sunk on the back side, which is 0.94 times or less the warp thickness in the base fabric thickness direction at the point where they are most raised on the front side.
[0019] Preferably, the warp yarns, which float above and below the weft yarn, have a thickness in the thickness direction of the base fabric at the point where they sink most deeply on the back side that is 0.70 to 0.90 times the thickness in the thickness direction of the base fabric at the point where they rise most deeply on the front side. Also preferably, in the above-mentioned flame-retardant surface fastener, the weft yarn is a combined yarn of a PPS multifilament yarn having a total thickness of 120 to 300 decitex, which is made up of 5 to 90 filaments having a thickness of 3 to 30 decitex, and a heat-fusible multifilament yarn having a total thickness of 80 to 150 decitex, which is made up of 15 to 40 polyester sheath-core filaments having a thickness of 3 to 8 decitex, the sheath component of which is a low-melting-point heat-fusible component.
[0020] Furthermore, in the above-mentioned flame-retardant hook-and-loop fastener, preferably, on the surface of the hook-and-loop fastener, engaging element regions where engaging elements are present and selvage regions where no engaging elements are present are each continuous in the warp direction, and the engaging element regions and selvage regions alternate in the weft direction, with multiple engaging element regions present, i.e., it is a wide hook-and-loop fastener before the selvage regions are slit to form multiple narrow hook-and-loop fasteners. Also preferably, the engaging elements are hook-shaped engaging elements, and the pull-out force of the hook-shaped engaging elements from the base fabric is 5 N or more. Also preferably, no backcoat resin layer is present on the back surface of the base fabric. Also preferably, it is colored with a pigment or disperse dye.
[0021] The present invention also provides a method for producing a flame-retardant hook-and-loop fastener, comprising: a base fabric woven from warp yarns composed of polyphenylene sulfide-based multifilament yarns; weft yarns composed of multifilament yarns composed of polyphenylene sulfide-based multifilament yarns and heat-fusible and heat-shrinkable filaments; and engaging element yarns composed of at least one type selected from the group consisting of polyphenylene sulfide-based multifilament yarns and monofilament yarns; and at least one type selected from the group consisting of a large number of hook-shaped engaging elements and a large number of loop-shaped engaging elements formed from the engaging element yarns, the method comprising carrying out the following steps A, B, C, and D in this order:
[0022] [Step A] When weaving a base fabric from warp and weft yarns, a step of weaving a loop fabric by weaving threads for engaging elements parallel to the warp yarns and at the same time regularly straddling the warp yarns and causing the threads for engaging elements to stand up in loops from the surface of the base fabric at the straddling points, [Step B] A step of guiding the loop fabric to a heating region and heating it to a temperature equal to or higher than the melting point of the heat-fusion component of the multifilament yarns made of heat-fusible and heat-shrinkable filaments and heat-shrinking the multifilament yarns made of heat-fusible and heat-shrinkable filaments, thereby fixing the threads for engaging elements to the base fabric with the melt from the multifilament yarns made of heat-fusible and heat-shrinkable filaments, [Step C] A step of removing the loop fabric from the heating region of Step B and sliding the back surface of the base fabric over a fixed surface or a roll surface while pressing it against the same surface while the heat-fusion component of the multifilament yarns made of heat-fusible and heat-shrinkable filaments is still molten, [Step D] A step of removing the loop fabric from step C, cooling the loop fabric, and then, if the thread for the engaging element is a monofilament thread, cutting one leg of the loop to form the loop into a hook-shaped engaging element;
[0023] In the method for producing such a flame-retardant hook-and-loop fastener, step C is preferably carried out by sliding the loop fabric over the fixed surface while pressing its back surface against the fixed surface, and changing the running direction of the loop fabric over the fixed surface. Also, step C is preferably carried out immediately after step B, without first cooling the loop fabric removed from step B, by utilizing the residual heat from step B.
[0024] In addition, in this method for producing a flame-retardant hook-and-loop fastener, the dry heat shrinkage rate at 200°C of the multifilament yarn made of heat-fusible and heat-shrinkable filaments is preferably in the range of 10 to 24%. Also preferably, the tension applied to the loop fabric in step C is 50 to 600 g / cm. Also preferably, steps A to D are performed continuously without winding up the fabric. Also preferably, in step A, a loop fabric is woven in which, on the surface of the loop fabric, engaging element regions where engaging element loops are present and selvage regions where no engaging element loops are present are each continuously present in the warp direction, and in which the engaging element regions and selvage regions are alternately present in the weft direction, with a plurality of engaging element regions present; and after step D, the centers of the selvage regions are slit in the warp direction, thereby simultaneously producing a plurality of hook-and-loop fasteners that are continuous in the warp direction and have selvage regions at both ends.
[0025] In the flame-retardant woven hook-and-loop fastener of the present invention, a heat-fusible and heat-shrinkable multifilament yarn is used as part of the weft yarn. When this yarn is heat-shrunk during heat fusion, it tightens the base of the engaging elements, preventing them from being pulled out of the woven base fabric. However, this causes vertical undulations on the hook-and-loop fastener, particularly in the width direction. As a result, it has been difficult to obtain a wide hook-and-loop fastener without undulations. This problem is solved in the present invention by performing step C after step B, i.e., after the heat fusion treatment, in which the back surface of the base fabric is pressed against a fixed surface or a roll surface and slid over the surface while the heat fusion component of the multifilament yarn made of the heat-fusible and heat-shrinkable filaments is still molten.
[0026] As a result, a wide, flame-retardant woven fabric hook-and-loop fastener with almost no waviness is obtained. Therefore, if the present invention is applied to a technique in which a wide hook-and-loop fastener is first manufactured and then slit parallel to the warp direction to simultaneously manufacture multiple narrow hook-and-loop fasteners, the center of the ear area can be accurately slit because the hook-and-loop fastener does not have waviness. In particular, if a method is used in step C in which the loop fabric is pressed against a fixed surface while sliding and running on the surface, and the running direction is changed on the fixed surface, the problem of waviness can be largely eliminated.
[0027] Furthermore, since the weft yarn contains heat-shrinkable yarn, the heat-shrunk yarn can tighten the base of the engaging elements, and the yarn for the engaging elements is fixed to the base fabric by the fusion of the heat-sealing component.Furthermore, in step C, the yarns (including the heat-sealing component) that make up the base fabric are pressed together and tightly adhered, and the molten heat-sealing component is pushed out of the weft yarn by the pressing, so that more of the molten material penetrates into adjacent yarns and the bonding strength between the yarns is increased.As a result, the engaging elements are firmly fixed to the base fabric, and further, the surface proportion of the heat-sealing component that impairs flame retardancy can be reduced.Therefore, even though the amount of heat-sealing component is small, the engaging elements are hardly pulled out of the base fabric even when engaging and peeling are repeated, and at the same time, with regard to flame retardancy, a hook-and-loop fastener with excellent flame retardancy can be obtained because the proportion of components that impair flame retardancy, i.e., the heat-sealing yarn, is low. In particular, in step C, by using a method in which the loop fabric is pressed against a fixed surface while sliding and running on the same surface, and the running direction is changed on the fixed surface, the proportion of heat-fusible threads is further reduced while the effect of preventing the engaging elements from being pulled out of the base fabric is further enhanced.
[0028] Furthermore, when the surface fastener is a hook surface fastener, since the vertical undulation of the base fabric is eliminated by step C, it is possible to reliably cut off one leg of the loop for the hook-shaped engaging element at the same height. This makes it possible to prevent a mixture of garments with both legs intact, both legs cut off, or even garments with one base cut off and one tip cut off, and as a result, it is possible to prevent a lack of excellent engaging force, variations in engaging force, and poor appearance.
[0029] Furthermore, in the flame-retardant hook-and-loop fastener of the present invention, the base fabric does not ripple in the vertical direction, so even if ears are provided at both ends along the warp direction, the ears do not meander, and the center can be sewn in with sewing thread in an attractive manner.
[0030] Furthermore, with the hook-and-loop fastener of the present invention, there is no need to apply a flame-retardant back coat resin liquid to the back surface of the hook-and-loop fastener base fabric as in conventional hook-and-loop fasteners, so there are no problems such as the back coat resin impairing the flexibility of the hook-and-loop fastener, or the back coat resin liquid lacking in stability, or the flame retardant added to the back coat resin liquid bleeding out and causing the flame retardancy to deteriorate over time.Furthermore, there are no problems such as the work environment being worsened by the solvent vapor of the back coat resin liquid when it is applied and dried, or the laborious application and drying process reducing productivity.
[0031] Fig. 1 is a diagram schematically showing an example of a heat treatment device in [Step B] that is preferably used when producing the flame-retardant surface fastener of the present invention, and an example of an apparatus that is preferably used in [Step C]. Fig. 2 is a diagram schematically showing a cross section of a preferred example of the flame-retardant surface fastener of the present invention, taken on a plane parallel to the warp yarns of the base fabric when [Step C] has been performed. Fig. 3 is a diagram schematically showing a cross section of a preferred example of the flame-retardant surface fastener of the present invention, taken on a plane parallel to the warp yarns of the base fabric when [Step C] has not been performed.
[0032] The present invention will be described in detail below. First, the PPS surface fasteners of the present invention can be broadly divided into three types: hook surface fasteners in which only hook-shaped engaging elements exist on the surface of a base fabric, loop surface fasteners in which only loop-shaped engaging elements exist on the surface of a base fabric, and hook-loop coexistence type surface fasteners in which hook-shaped engaging elements and loop-shaped engaging elements exist side by side on the surface of a base fabric. The present invention is directed to these three types of surface fasteners.
[0033] Of these, hook surface fasteners are mainly formed from monofilament yarns for hook-shaped engaging elements, multifilament yarns for warp, and multifilament yarns for weft. Loop surface fasteners are mainly formed from multifilament yarns for loop-shaped engaging elements, multifilament yarns for warp, and multifilament yarns for weft. Hook-loop coexisting surface fasteners, in which hook-shaped engaging elements and loop-shaped engaging elements coexist on the same surface, are mainly formed from monofilament yarns for hook-shaped engaging elements, multifilament yarns for loop-shaped engaging elements, multifilament yarns for warp, and multifilament yarns for weft. These surface fasteners may, if necessary, have a small amount of yarns other than those mentioned above woven into them, or may not have any yarns other than those mentioned above woven into them.
[0034] In the present invention, the warp yarns and the yarns for the engaging elements must both be yarns made of a PPS resin, since these yarns provide excellent flame retardancy, have excellent fiber properties and weavability, and can be bonded by thermal fusion with a thermal adhesive component. Therefore, PPS multifilament yarns are used for the warp yarns, PPS multifilament yarns for the yarns for the loop-shaped engaging elements, and PPS monofilament yarns for the yarns for the hook-shaped engaging elements. Furthermore, in the present invention, PPS multifilament yarns are used as the main yarns constituting the weft yarns to further enhance flame retardancy.
[0035] PPS resin is a resin that is flame retardant and has excellent heat resistance, as well as excellent fiber formability and fiber physical properties. The PPS multifilament yarn and PPS monofilament yarn used in the present invention are obtained from PPS resin having a weight-average molecular weight of 20,000 to 100,000, i.e., by melt-spinning, stretching, and optionally heat-treating this PPS resin. Various types of such PPS multifilament yarn and PPS monofilament yarn are currently commercially available, and fiber manufacturers manufacture and provide yarns with desired thicknesses and fiber counts to meet user demands. Furthermore, PPS multifilament yarns and monofilament yarns may contain flame retardants, colorants, various stabilizers, and even small amounts of other resin components, as long as they do not interfere with flame retardancy, fiber properties, or weavability.
[0036] As the warp yarn used in the present invention, a PPS multifilament yarn having a total thickness of 150 to 350 decitex, composed of 24 to 90 PPS filaments having a thickness of 2 to 10 decitex, is preferred, as it covers the surface of the multifilament yarn composed of heat-fusible and heat-shrinkable filaments used as part of the weft (hereinafter sometimes referred to as heat-fusible yarn), enhances the bonding by the heat-fusible yarn, and achieves a higher level of flame retardancy. A more preferred warp yarn is a PPS multifilament yarn having a total thickness of 200 to 300 decitex, composed of 30 to 80 PPS filaments having a thickness of 3 to 8 decitex. From the viewpoint of weaving, it is preferable that such PPS multifilament yarn has a twist of 100 to 800 T / m, more preferably 300 to 600 T / m. Note that T / m stands for turns / meter.
[0037] The weft yarn is preferably a yarn mainly composed of a PPS multifilament yarn and a heat-sealed yarn, and particularly preferably a yarn obtained by aligning these two. Among these, a aligning yarn is preferred, which is composed of a PPS multifilament yarn having a total thickness of 120 to 300 decitex, which is made up of 5 to 90 PPS filaments having a thickness of 3 to 30 decitex, and a multifilament yarn having a total thickness of 80 to 150 decitex, which is made up of 15 to 40 polyester sheath-core filaments having a thickness of 3 to 8 decitex, the sheath component of which is a low-melting-point heat-sealed component, and in which the total decitex of the PPS multifilament yarn is greater than the total decitex of the heat-sealed yarn.
[0038] Among these paralleled yarns, it is particularly preferable that the weft yarn is a paralleled yarn of a PPS multifilament yarn having a total thickness of 140 to 280 decitex, in which 6 to 80 filaments having a thickness of 3.5 to 24 decitex are bundled together, and a multifilament yarn having a total thickness of 80 to 140 decitex, in which 20 to 30 polyester sheath-core filaments having a thickness of 3 to 6 decitex are bundled together, in which the sheath component is a low-melting point heat-fused component.
[0039] In particular, when a wide hook-and-loop fastener is manufactured and then slit to simultaneously manufacture a plurality of narrow hook-and-loop fasteners, in order to prevent fraying from the slit portions, it is preferable to use as the weft a drawn yarn of a PPS multifilament yarn having a total thickness of 150 to 280 decitex, in which 8 to 80 filaments having a thickness of 3.5 to 20 decitex are bundled together, and a multifilament yarn having a total thickness of 80 to 140 decitex, in which 20 to 30 polyester core-sheath filaments having a thickness of 3 to 6 decitex are bundled together, the sheath component of which is a low-melting point heat-fusible component.
[0040] On the other hand, when a narrow or wide hook-and-loop fastener is produced directly from the weaving process without slitting, it is preferable to use as the weft a combined yarn of a PPS multifilament yarn having a total thickness of 140 to 200 decitex, which is made up of 6 to 20 bundled filaments having a thickness of 10 to 24 decitex, and a multifilament yarn having a total thickness of 80 to 140 decitex, which is made up of 20 to 30 bundled polyester core-sheath filaments having a thickness of 3 to 6 decitex, the sheath component of which is a low-melting point heat-fused component, in order to improve the appearance quality.
[0041] Furthermore, it is preferable that the heat-fusion yarn constituting a portion of the weft yarn maintains its thread shape even after heat fusion in terms of heat fusion performance, and ultimately in terms of the performance of the hook-and-loop fastener after heat fusion. Therefore, a multifilament yarn consisting of a sheath-core filament in which the heat-fusion component forms a sheath component exposed on the fiber surface and the core component does not melt at the heat fusion temperature is preferred as the heat-fusion yarn. The sheath component, which is part of this sheath-core filament, melts at a temperature of 240°C or less, and this molten material adheres and fixes the nearby PPS-based engaging element yarn and warp yarn. For heat-fusion yarn, a sheath component made of a polyester-based resin is preferred in terms of adhesion to PPS-based multifilament yarns and monofilament yarns, water absorption stability, thermal stability, yellowing resistance, etc.
[0042] In particular, from the viewpoints of ease of handling and adhesiveness during heat fusion, and resistance to peeling between the core and sheath components, multifilament yarns made of filaments with a core-sheath cross section are preferred, with the sheath component being a low-melting point polyester resin and the core component being a high-melting point polyester resin that does not melt at the temperature at which the sheath component is heat fused. Specifically, the sheath component is preferably a polyethylene terephthalate copolymer having a melting point of 220°C or less, particularly 120 to 210°C, obtained by copolymerizing copolymer components such as isophthalic acid, sulfoisophthalic acid, adipic acid, and propylene glycol.
[0043] The core component is preferably a polyester with a high melting point, specifically a polyester that is not copolymerized, or a polyester that is copolymerized but has a melting point 50 to 120°C higher than that of the sheath component resin, such as a polyethylene terephthalate homopolymer or a polyethylene naphthalate homopolymer.
[0044] The cross-sectional shape of the sheath-core filament may be single-core or multi-core, and may be concentric or eccentric. It may also have a bimetallic cross section. In other words, it is sufficient if the low-melting point component is exposed on the fiber surface. The weight ratio of the core component to the sheath component is preferably in the range of 75 / 25 to 30 / 70, and particularly preferably in the range of 80 / 20 to 55 / 45.
[0045] In particular, in the present invention, the heat-sealing yarn preferably has heat shrinkability in order to enhance the pull-out resistance of the engaging elements. Specifically, a yarn having a dry heat shrinkage rate of 10 to 24% at 200°C is used. More preferably, a dry heat shrinkage rate of 12 to 22% at 200°C is used. Furthermore, with regard to the PPS yarns used for the warp, engaging element yarns, and weft yarns, heat shrinkability is preferred in terms of the pull-out resistance of the engaging elements. Specifically, in the case of PPS-based multifilament yarns used for the warp, weft, and loop-shaped engaging element yarns, a dry heat shrinkage rate of 3 to 15% at 200°C is preferred, and in the case of monofilament yarns used for hook-shaped engaging element yarns, a dry heat shrinkage rate of 1 to 4% is preferred. The dry heat shrinkage rate at 200°C referred to here is the value calculated from the shrunk yarn after leaving a 50 cm length of yarn in a free state in an atmosphere at 200°C for one minute, and is the average value measured for ten randomly selected yarns.
[0046] The weight ratio of the PPS multifilament yarn to the heat-fusible yarn constituting the weft is preferably in the range of 80:20 to 52:48 in terms of achieving both flame retardancy and the ability to fix the engaging elements, and more preferably in the range of 75:25 to 55:45. In particular, when a wide hook-and-loop fastener is produced and then slit to produce multiple narrow hook-and-loop fasteners at the same time, the range of 75:25 to 60:40 is preferred, and when narrow or wide hook-and-loop fasteners are produced directly from the weaving process without slitting, the range of 70:30 to 55:45 is preferred.
[0047] In this way, the yarn made of PPS multifilament yarn and heat-sealing yarn used as the weft yarn is preferably in a so-called non-twisted state, with a twist of 0 to 80 T / m, because this allows the heat-sealing resin of the sheath component to function effectively and firmly fix the engaging element yarn. In the present invention, the warp yarn, weft yarn, and engaging element yarn may be mixed with small amounts of other filaments within a range that does not impair the flame retardancy, engaging force, or performance when stored under high-temperature and high-humidity conditions for a long period of time of the hook-and-loop fastener.
[0048] As the PPS-based monofilament yarn used for the hook-shaped engaging element, from the viewpoint of engaging force and because the hook shape is not stretched even when engaging and releasing are repeated, a monofilament yarn made of a PPS-based resin and having a diameter of 150 to 250 μm is preferred, a monofilament yarn having a diameter of 180 to 220 μm is more preferred, and a monofilament yarn having a diameter of 195 to 210 μm is particularly preferred.
[0049] Furthermore, as the PPS-based multifilament yarn used as the loop-shaped engaging element, in terms of engaging force, the engaging element is less likely to break due to repeated engagement and peeling, and the surface of the hook-and-loop fastener is soft to the touch, a PPS-based multifilament yarn having a total thickness of 200 to 500 decitex, which is made by bundling 8 to 30 filaments, also made of PPS-based resin, each having a thickness of 8 to 30 decitex, is preferred, and a PPS-based multifilament yarn having a total thickness of 250 to 450 decitex, which is made by bundling 16 to 24 filaments, each having a thickness of 12 to 20 decitex, is particularly preferred.
[0050] In general hook-and-loop fasteners, multifilament yarns consisting of 8 to 15 filaments are usually used as the yarns for the loop-shaped engaging elements, but in the flame-retardant hook-and-loop fastener of the present invention, it is preferable to use multifilament yarns with a greater number of filaments as the yarns for the loop-shaped engaging elements, which allows the surface of the base fabric to be densely covered with PPS-based loop-shaped engaging elements, thereby making it possible to further improve flame retardancy.Furthermore, it is preferable that the yarns for the loop-shaped engaging elements be untwisted multifilament yarns, so that when they are used as engaging elements, the multifilament yarns will unravel and improve the engaging force.
[0051] A woven fabric flame-retardant surface fastener is manufactured from such warp yarns, weft yarns, and threads for engaging elements by sequentially carrying out the above-mentioned steps A to D. Next, the manufacturing method of the woven fabric flame-retardant surface fastener will be explained in the order of these steps.
[0052] First, a woven fabric having a large number of loops for engagement elements on its surface is woven by the following step A. [Step A] When weaving a base fabric from warp and weft yarns, the threads for engagement elements are woven parallel to the warp yarns, and at the same time, the threads for engagement elements are regularly made to cross the warp yarns, and the threads for engagement elements are made to stand up in loops from the surface of the base fabric at the crossing points, thereby weaving a loop woven fabric.
[0053] As the weave structure when weaving a loop fabric by this process A, a plain weave is preferred in which monofilament yarns for hook-shaped engaging elements and multifilament yarns for loop-shaped engaging elements are used as part of the warp yarns, and these engaging element yarns are woven parallel to the warp yarns, causing three weft yarns to float and sink and rise from the surface of the base fabric.In the case of a hook surface fastener, a weave structure in which the yarns form a loop, stepping over one to three warp yarns, or slipping between the warp yarns, causing three weft yarns to float and sink is preferred because this makes it easy to efficiently cut one leg of the hook engaging element loop, and in the case of a loop surface fastener, a weave structure in which the yarns form a loop, stepping over one warp yarn, and slipping between the warp yarns is preferred because this makes it easy to fix the engaging element to the base fabric. In particular, a weave in which the loop for the hook-shaped engaging element and the loop for the loop-shaped engaging element both float up and down over three weft threads to form a loop while stepping over one warp thread and slipping between the warp threads is preferred, as this provides excellent resistance to the pulling out of the engaging elements and also allows the engaging elements to easily stand up facing the same direction, resulting in an even higher engaging force.
[0054] Generally, in the case of hook surface fasteners, the thread for the hook-shaped engaging element crosses two or three warp threads, at which point a loop for forming the hook-shaped engaging element is formed, and in the case of loop surface fasteners, the loop is formed without crossing the warp thread, which is adopted for ease of production and ease of engagement between the hook-shaped engaging element and the loop-shaped engaging element. However, in the present invention, it is preferable to use a method that differs from this general crossing method, in which the loops of both the hook-shaped engaging element and the loop-shaped engaging element are formed at a point where they cross one warp thread.
[0055] The same is true for hook-and-loop coexisting surface fasteners, and it is preferable that the threads for the hook-shaped engaging elements and the threads for the loop-shaped engaging elements are woven between the warp threads so that two adjacent threads sandwiching the warp threads are the same thread for the engaging elements.In this case, the ratio of the number of monofilament threads for the hook-shaped engaging elements to the number of multifilament threads for the loop-shaped engaging elements is preferably in the range of 40:60 to 60:40.
[0056] The weave density of the woven fabric is preferably 50 to 90 warp threads / cm (including threads for the engaging elements), particularly 55 to 80 warp threads / cm, and 10 to 30 weft threads / cm, particularly 12 to 24 weft threads / cm.The proportion of heat-fusible threads in the entire hook-and-loop fastener is preferably 5 to 15% by weight, particularly 6 to 10% by weight, from the viewpoint of achieving both flame retardancy and pull-out resistance of the engaging elements.
[0057] Furthermore, the height of the hook-shaped engaging elements of the surface fastener is preferably 1.2 to 2.0 mm from the surface of the base fabric, and the height of the loop-shaped engaging elements is preferably 1.9 to 3.0 mm from the surface of the base fabric, from the viewpoint of the engaging force and the difficulty of the engaging elements falling over.
[0058] The density of hook-shaped engaging elements in a hook surface fastener, the density of loop-shaped engaging elements in a loop surface fastener, and the total density of hook-shaped engaging elements and loop-shaped engaging elements in a hook-loop coexisting surface fastener are each 40 to 80 pieces / cm based on the base fabric portion where the engaging elements exist and on the area after heat shrinkage. 2 , 40-80 pieces / cm 2 , 40-80 pieces / cm 2 are preferred, and in particular, 45 to 75 particles / cm 2 , 45-75 pieces / cm 2 , 45-75 pieces / cm 2 Thus, it is preferable for the surface of the surface fastener to be covered with many PPS-based engaging elements in order to enhance flame retardancy. In the hook-and-loop coexistence type surface fastener, the ratio of the number of hook-shaped engaging elements to the number of loop-shaped engaging elements is preferably in the range of 40:60 to 60:40.
[0059] In addition, when forming loops for hook-shaped engaging elements, in order to facilitate the formation of loops for hook-shaped engaging elements of uniform height, it is preferable to use a method in which metal rods having uniform longitudinal cross sections are placed in a row in the same number as the number of threads for the engaging elements, parallel to the warp threads, at the position where the threads for the hook-shaped engaging elements straddle the warp threads, with the cross sections oriented in the height direction, and the threads for the engaging elements are straddled over the top of these metal rods to form loops of the same shape, and after the loops are formed, the metal rods are pulled out of the loops.
[0060] In the above step A, selvage regions where no engaging element loops are present on the surface may be provided at both ends of the loop fabric in the warp direction, and selvage regions (middle ear regions) where no engaging element loops are present on the surface may also be provided other than at both ends. Since the present invention is particularly suited to the manufacture of wide loop fasteners, it is preferred to use it in a method for simultaneously manufacturing a wide loop fabric in which engaging element regions and middle ear regions are present on the surface of the wide loop fabric, each continuously in the warp direction, and engaging element regions and middle ear regions are alternately arranged in the weft direction, with a plurality of engaging element regions present, and then, after the above step D, the center of the middle ear region is slit in the warp direction to form a hook-and-loop fastener having selvage regions at both ends of a plurality of continuous lines in the warp direction (at least one of the selvage regions originates from the middle ear region).
[0061] The width of the engaging element region having the ears is preferably 10 to 50 mm, the width of the ear regions provided at both ends is preferably 1.5 to 4 mm, and in the case of the middle ear region, the width of the ear region is preferably 3 to 8 mm. When the middle ear region of a wide hook-and-loop fastener is slit to simultaneously produce multiple hook-and-loop fasteners, the number of narrow hook-and-loop fasteners obtained by slitting is preferably 2 to 10, and the width of the hook-and-loop fastener before slitting is preferably 50 to 300 mm.
[0062] When a middle ear region is provided, after step D, a method is used in which the center of the middle ear region is slit and a narrow hook-and-loop fastener tape is obtained at the same time.In the case of the flame-retardant hook-and-loop fastener of the present invention, since there is almost no waviness in the vertical direction, the center of the middle ear region can be slit accurately, and multiple hook-and-loop fasteners can be obtained at the same time, with ears of a constant width at both ends that continue in a straight line without meandering in the warp direction.
[0063] The loop fabric for hook-and-loop fasteners thus obtained is then sent to the following step B, where it is subjected to a heat treatment to melt the heat-fusible component which is the sheath component of the heat-fusible yarn. [Step B] A step in which the loop fabric obtained in step A is introduced into a heating zone, heated to a temperature at which the heat-fusible component of the heat-fusible yarn melts or higher, and the heat-fusible yarn is thermally shrunk, so that the rising portions of the loops made of the yarn for engaging elements are fixed to the base fabric by the molten material from the heat-fusible yarn.
[0064] Preferably, the loop fabric produced in step A is heat-treated immediately after step A without being wound up, so that the loop fabric runs continuously in a long state through a heat treatment furnace (3) as shown in Fig. 1. This heat treatment melts the sheath component of the heat-fusible yarn that constitutes the weft yarn and simultaneously causes it to shrink, fixing the monofilament or multifilament yarn for the engaging element to the base fabric. It is preferable that the long fabric for a hook-and-loop fastener running through the heat treatment furnace be run without applying too much tension in the width direction so that it can shrink sufficiently.
[0065] This eliminates the need for the application of a backcoat adhesive and the drying process required for conventional woven surface fasteners, thereby preventing the aforementioned process and performance problems associated with backcoat adhesives. Furthermore, the heat generated during this heat treatment fixes the loop shape of the hook-shaped engaging elements, so that even after one leg of the loop for the hook-shaped engaging element is cut off to form the hook-shaped engaging element in the subsequent step D, the hook shape is maintained and sufficient engaging strength is obtained. Furthermore, in the case of loop-shaped engaging elements, the heat generated during this heat treatment also results in a natural, uniform loop shape.
[0066] The temperature used in the heat treatment step B is 230 to 260°C, which is a temperature at which the heat-fusible components constituting the weft yarn melt or soften but other components and yarns do not melt, and at which the monofilament yarn for the hook-shaped engaging element is fixed in a loop shape, and is more preferably in the range of 240 to 258°C. Such heat treatment is usually carried out by running the fabric for the hook-and-loop fastener through a heated oven. Specifically, the heat treatment is completed by running the fabric through the heating oven at a speed of 0.30 to 1.30 m / min for 20 to 120 seconds.
[0067] The loop fabric in which the heat-fusible component of the heat-fusible yarn has been melted and the molten resin has penetrated into the adjacent yarns is then subjected to the following step C. [Step C] A step of removing the loop fabric from the heating zone of step B, and sliding the back surface of the base fabric on a fixed surface or a roll surface while pressing the back surface of the base fabric on the surface while the heat-fusible component of the heat-fusible yarn is still molten.
[0068] That is, in the step B, when the heat-treated fabric for a hook-and-loop fastener leaves the heat treatment furnace (3), as shown in Fig. 1, while the heat-fusible component of the heat-fusible yarn remains molten, the back surface of the base fabric (1) is pressed against a fixed surface or roll surface (4) and slid across the surface. Fig. 1 shows a case where the back surface of the fabric for a hook-and-loop fastener (1) is pressed against the fixed surface (4) and slid across the surface immediately after leaving the heat treatment furnace (3).
[0069] This process C can eliminate the vertical undulation of the hook-and-loop fastener, resulting in a wide, flat, flame-retardant hook-and-loop fastener with almost no undulation. Furthermore, this process can further prevent the engaging elements from being pulled out of the base fabric even when the engaging and releasing processes are repeated. That is, this process presses the threads constituting the base fabric together, and the heat-sealing component pushed out by the press-bonding penetrates into the adjacent threads, further increasing the bonding strength and firmly fixing the engaging elements to the base fabric, thereby reducing the proportion of the heat-sealing component. As a result, even with a small amount of the heat-sealing component, the engaging elements can be prevented from being pulled out of the base fabric. At the same time, with regard to flame retardancy, the proportion of the heat-sealing component that impairs flame retardancy can be reduced, resulting in a hook-and-loop fastener with excellent flame retardancy.
[0070] In the present invention, the PPS-based yarns used as warp yarns, engaging element yarns, and also as part of the weft yarns are much stiffer than yarns made of ordinary synthetic fibers, so simply pressing the back surface of a loop fabric made of such yarns against a fixed surface or a roll surface makes it difficult to achieve the above-mentioned effect, but if step C is performed by pressing the loop fabric against a fixed surface or a roll surface and sliding it on the same surface, the above-mentioned effect can be achieved to a high extent. In other words, in the case of a PPS-based hook-and-loop fastener, even if the loop fabric is brought into contact with the surface of a roll rotating at the same surface speed as the running speed of the fabric, it will not slide on the same surface, and therefore no effect can be expected.
[0071] In other words, it is necessary to satisfy all of the following requirements: the back surface of the loop fabric is pressed against a fixed surface or a roll surface, and the loops for the engaging elements present on the surface opposite to the pressed surface are not pressed down by the same operation; and the running loop fabric is allowed to slide on a fixed surface (4) or on a roll surface rotating at a surface speed different from the running speed of the loop fabric (1).
[0072] In this way, by sliding the warp filaments over the surface while being pressed against a fixed surface or a roll surface, the movement of the warp filaments to a stable position is promoted, and accordingly the weft also settles to a natural state and the shrinkage state becomes uniform, thereby eliminating distortion and promoting the squeezing out of the heat-fused components from the weft. By sliding the warp filaments over the surface while being pressed against the fixed surface or a roll surface, the thickness of the warp filaments at the most sunken position on the back surface, which is located above and below the weft, as will be described later, in the thickness direction of the base fabric, satisfies the condition of 0.94 times or less the warp thickness at the most raised position on the front surface.
[0073] Furthermore, to achieve this state, as described below, it is preferable to apply a tension of about 50 to 600 g / cm to the loop fabric while changing the running direction of the loop fabric after it comes into contact with the fixed surface or roll surface. A tension of about 100 to 400 g / cm is more preferable. In the present invention, step C is preferably performed by changing the running direction of the loop fabric while pressing it against the fixed surface or roll surface and sliding it on the surface. Changing the running direction facilitates pressing the loop fabric against the fixed surface or roll surface and improves the effect of pressing and sliding it against the fixed surface or roll surface.
[0074] Furthermore, it is preferable to carry out the above step C on the loop fabric removed from step B without first cooling it, immediately following step B, while the loop fabric is still maintained at a high temperature due to the heat applied in step B, i.e., by using the residual heat from step B. Even if the loop fabric is cooled after passing through step B and then reheated, a certain degree of effect can be expected, but distortion in the loop fabric that has been cooled and fixed is difficult to eliminate, making it difficult to fully achieve the effects of the present invention. Therefore, it is preferable to carry out step C on the fabric for hook-and-loop fasteners removed from step B, immediately, near the location where step B was carried out.
[0075] It is preferable that the front and back surfaces of the loop fabric for hook-and-loop fasteners sent to this step do not come into contact with any solid object such as a roller or guide at all after entering the heat treatment furnace (3) until the back surface is pressed against the fixed surface or roll surface (4), and that the fixed surface or roll surface is the first object with which the fabric comes into contact.
[0076] In the present invention, the fixed surface or roll surface (4) used in step C preferably has a contact length with the backing fabric of 20 to 100 mm and a contact time of 2 to 10 seconds. Specific examples of suitable surfaces include fixed surfaces and roll surfaces made of metal, ceramic, or heat-resistant resin. The surface of the fixed surface or roll surface may be mirror-finished or matte, or may have some irregularities as long as it can press down the back side of the loop fabric and allow the back side of the loop fabric to slide. The running speed when sliding over the fixed surface or roll surface (4) is preferably 5 to 22 mm / sec.
[0077] When a roll surface is used in step C, as described above, it is preferable to make a difference between the surface speed of the roll and the running speed of the loop fabric pressed against that surface, and to run the loop fabric while sliding it on the same surface. In this case, the speed difference between the surface speed of the roll and the loop fabric running on the roll surface is preferably 10 to 100 mm / sec. Furthermore, as shown in Figure 1, it is particularly effective to have the back surface of the fabric shaped so that the running direction changes 30 to 180 degrees along the fixed surface. In Figure 1, the fabric for hook-and-loop fasteners (1) changes its running direction by 90 degrees along the fixed surface (4).
[0078] In order to enhance the contact effect, it is preferable that such a fixed surface or roll surface (4) be heated to a temperature 80 to 180°C lower than the heat treatment temperature. However, it is usually sufficient to warm the surface of the fixed surface or roll surface (4) using the residual heat of the base fabric (1) upon exiting the heat treatment furnace. The surface pressing the backside of the base fabric may be either a fixed surface, a roll surface whose contact surface rotates at a surface speed different from that of the base fabric as the base fabric travels, or a driven roll surface that actively pulls the base fabric and rotates at a surface speed different from that of the base fabric. However, in the case of a roll surface, as described above, it is necessary to create a difference between the surface speed of the roll and the running speed of the loop fabric traveling while being pressed against its surface, so that the backside of the loop fabric slides over the roll surface. Therefore, a fixed surface such as that shown in Figure 1 is preferred because it is structurally simple and easily effective. A narrow guide-shaped surface may also be used, but a fixed surface having the contact length described above is preferred.
[0079] In the present invention, as shown in Figure 1, the base fabric (1) is run through a heat treatment furnace (3), where the weft yarn is shrunk as described above, and then exits the heat treatment furnace (3) and continues running over a fixed surface (4). As a result, the base fabric (1) is subjected to tension in the warp direction while being pressed against the fixed or roll surface (4). To enhance the effect, it is preferable that the tension applied to the base fabric immediately after passing through the fixed surface (4) is about 50 to 600 g / cm. More preferably, it is about 100 to 400 g / cm.
[0080] In the case of the woven surface fastener of the present invention, the warp yarns float above and below the weft yarns, sandwiching them, so that the back surface of the base fabric is covered with the warp yarns, and therefore the weft yarns containing the heat-fusible component hardly come into direct contact with the fixed surface or the roll surface 4. Therefore, there is almost no risk of the molten heat-fusible component directly adhering to the fixed surface or the roll surface 4, which would otherwise cause problems.
[0081] As described above, the operation of sliding the hook-and-loop fastener fabric (1) while pressing its back surface against a fixed surface or roll surface (4) in a state in which the heat-fusion component constituting the weft yarn is molten is preferably carried out by utilizing the residual heat from the heat treatment so as to continue with the heat treatment in the heat treatment furnace (3) as shown in Figure 1 without first cooling the hook-and-loop fastener fabric heat-treated in step B, in order to enhance the effects of the present invention and in terms of productivity. However, it is also possible to remove the hook-and-loop fastener fabric from the heat treatment furnace (3), cool it once, and then reheat the back side of the base fabric to melt the heat-fusion component of the weft yarn on the back side of the hook-and-loop fastener fabric, and then press it against a fixed surface or roll surface (4) in this state, but the effect obtained will be less.
[0082] By performing the operation [Step C] of pressing the back surface of the base fabric (1) against a fixed surface or roll surface (4) while sliding it on the same surface while the heat-fusible component is molten, as shown in Figure 2, the thickness (Tb) of the warp threads, which are floating above and below the weft thread and are sandwiched between the weft thread and the base fabric thickness direction at the point where they are most deeply sunk on the back surface, in the thickness direction of the base fabric is 0.94 times or less than the warp thickness (Ts) of the warp threads, which are most deeply sunk on the front surface and are sandwiched between the weft thread and the base fabric thickness direction at the point where they are most deeply sunk on the front surface and are most deeply sunk on the front surface, in the thickness direction of the base fabric. In particular, by sliding the warp threads on the same surface while pressing them against a fixed surface and changing the running direction as described above, the thickness of the warp threads, which are floating above and below the weft thread and are sandwiched between the weft thread and the base fabric thickness direction at the point where they are most deeply sunk on the back surface and are sandwiched between the weft thread and the base fabric thickness direction at the point where they are most deeply sunk on the front surface and are most deeply sunk on the front surface and are less than 0.90 times the warp thickness in the thickness direction of the base fabric. Note that in Figures 2 and 3, K indicates the thickness direction of the base fabric.
[0083] However, if (Tb) is too low, the back surface of the hook-and-loop fastener base fabric will become dense and flat due to heat fusion, and the flexibility, texture, and even breathability and liquid permeability that are the advantages of a woven base fabric will be lost, which is not desirable.Therefore, it is preferable that (Tb) be 0.7 times or more, and particularly 0.75 times or more, of (Ts).
[0084] Fig. 2 shows a cross-sectional view of a woven surface fastener in which the effect of the present invention can be achieved by pressing the back surface of the base fabric (1) against a fixed or rolled surface (4) while the heat-sealing component is molten and sliding the fastener on the same surface, i.e., when (Tb) is 0.94 times or less than (Ts) (hereinafter, this may also be expressed as the (Tb) / (Ts) ratio or the ratio of (Tb) to (Ts)).On the other hand, Fig. 3 shows a cross-sectional view of a woven surface fastener in which the back surface of the base fabric (1) is not pressed against a fixed or rolled surface (4) while the heat-sealing component is molten, and in this case, (Tb) is almost the same value as (Ts), and the (Tb) / (Ts) ratio of 0.94 or less as described above is not satisfied.
[0085] Even if the operation of pressing the back surface of the base fabric against a fixed surface or a roll surface while sliding it on the same surface while the heat-sealing component is molten, i.e., [Step C], is not performed, the value of (Tb) may become slightly smaller than the value of (Ts) due to the natural gravity of the hook-and-loop fastener during the manufacturing process of the hook-and-loop fastener fabric, but the decrease is extremely small, and (Tb) will never become less than 0.96 times (Ts).
[0086] Next, we will explain how to measure the thicknesses (Tb) and (Ts) of the warp threads that float above and below the weft thread. First, select a region where the engaging elements are present on the surface and are least affected by the engaging elements. Then, cut the hook-and-loop fastener parallel to the warp threads using a safety razor blade as a cutting device, cutting through the center of the warp bulge. The resulting cross section is then photographed at 200x magnification. Figure 2 shows a schematic representation of the resulting cut section. From this photograph, three locations where the warp threads are most deeply sunk on the back side are randomly selected, and three locations where they are most raised on the front side are also randomly selected, and the thickness in the thickness direction of the base fabric at each location is measured. Similar measurements are performed at 10 random locations on the hook-and-loop fastener, and the thickness in the thickness direction of the base fabric at each location is measured. Of the 30 thickness measurements taken for the base fabric thickness direction at the point where the fabric is most sunken on the back side and the 30 thickness measurements taken for the point where the fabric is most raised on the front side, the five highest and five lowest measurements are removed, and the average values of the remaining 20 are calculated. The average values thus obtained are the warp thickness (Tb) in the base fabric thickness direction at the point where the fabric is most sunken on the back side and the warp thickness (Ts) in the base fabric thickness direction at the point where the fabric is most raised on the front side.
[0087] It should be noted that even if the hook-and-loop fastener fabric is pressed against a fixed surface or a roll surface while the heat-fusible component of the weft yarns is still in a molten state, not all of the warp yarns present on the back surface of the hook-and-loop fastener fabric that are most deeply sunk on the back surface side will be pressed against the fixed surface or the roll surface, and there may be some locations that are not pressed against the fixed surface or the roll surface and where the thickness (Tb) of the warp yarns on the back surface side is almost the same as the thickness (Ts) on the front surface side, but in the present invention, such locations are also included in the arbitrarily selected locations. Therefore, it can be said that the (Tb) / (Ts) ratio specified in the present invention is an average value obtained including these locations.
[0088] On the other hand, Figure 3 shows the case where the hook-and-loop fastener fabric is not pressed against the fixed surface or roll surface as described above. In a case like Figure 3, i.e., when (Tb) and (Ts) are almost the same value, the effect obtained by using process C, namely, reducing the occurrence of undulations in the vertical direction of the hook-and-loop fastener and further highly preventing the engaging elements from being pulled out of the base fabric due to repeated engagement and peeling, cannot be obtained.
[0089] In the present invention, the ratio of (Tb) to (Ts) is mainly determined by the strength of pressing when the hook-and-loop fastener base fabric is pressed and slid against a fixed surface or roll surface, and therefore this value can be freely changed by sliding the hook-and-loop fastener base fabric over the fixed surface or roll surface while applying tension, and changing the running direction along the fixed surface or roll surface as shown in Figure 1.
[0090] In the present invention, when the back surface of the hook-and-loop fastener base fabric is pressed against a fixed surface or roll surface while the heat-fusible component constituting the weft yarn remains molten, it is necessary not to press the front surface of the hook-and-loop fastener base fabric on which the hook-and-loop fastener engagement element loops are present against the fixed surface or roll surface. In other words, if the hook-and-loop fastener base fabric is sandwiched between rolls and pressed down from above and below, the engagement element loops that are upright on the surface of the base fabric will be pressed down by the pressure from above and will be fixed to the surface of the base fabric in that state, which will reduce the engagement ability of the hook-and-loop fastener and also worsen the appearance of the hook-and-loop fastener. Furthermore, if both the front and back sides of the hook-and-loop fastener base fabric are pressed against a fixed surface or roll surface, (Tb) and (Ts) will be approximately equal, and the (Tb) / (Ts) ratio of 0.94 or less specified in the present invention will not be satisfied.
[0091] Next, if the loops for the engaging elements are loops for hook-shaped engaging elements, the woven fabric having the loops for the engaging elements obtained in this way on its surface is sent to the following step D, where one leg of the loop for the hook-shaped engaging element is cut to form a hook-shaped engaging element. [Step D] A step of pulling out the loop fabric from step C, cooling the loop fabric, and then, if the thread for the engaging element is a monofilament thread, cutting one leg of the loop to form the loop into a hook-shaped engaging element.
[0092] The cutting device used for this purpose is preferably one having a structure in which one leg of the loop for the hook-like engaging element of the base fabric for a hook surface fastener or a base fabric for a hook-and-loop co-existing type surface fastener running in the warp direction is cut by the reciprocating motion of a movable cutting blade between two fixed blades.The woven fabric from which one leg of the loop for the hook-like engaging element has been cut is used as a hook surface fastener or a hook-and-loop co-existing type surface fastener.
[0093] Furthermore, since the loop fabric emerging from process C does not have a base fabric that ripples in the vertical direction, in the next process D, it is possible to reliably cut off one leg of the loop for the hook-shaped engaging element at approximately the same height, preventing the occurrence of fabrics with both legs not cut or both legs cut, or even a mixture of fabrics with cuts near the base of one leg and fabrics with cuts near the tip of one leg, thereby preventing variations in the engaging force and preventing the appearance of the hook-and-loop fastener from being impaired.
[0094] According to the present invention, a flame-retardant woven surface fastener is obtained which has excellent resistance to the engaging elements being pulled out of the base fabric by repeated engagement and release, despite the fact that the proportion of heat-fused yarns which impair flame retardancy is small. In particular, when the engaging elements are hook-shaped engaging elements, it has been extremely difficult to achieve pull-out resistance of the hook-shaped engaging elements from the base fabric without impairing flame retardancy; however, according to the present invention, pull-out resistance of the hook-shaped engaging elements from the base fabric is achieved with a pull-out force of 5N or more.
[0095] Furthermore, conventional flame-retardant hook-and-loop fasteners lack flexibility when a backcoat resin layer is present on the back surface, and when heat-sealable and heat-shrinkable weft yarns are used to impart pull-out resistance to the engaging elements, the heat-sealing process causes undulations in the vertical direction, making it difficult to manufacture commercially valuable wide flame-retardant hook-and-loop fasteners.However, the present invention makes it possible to obtain a wide hook-and-loop fastener with a flat surface that does not undulate in the vertical direction.
[0096] The present invention is particularly suitable for producing hook-and-loop fasteners with a width of 15 to 200 mm in the weft direction and no vertical undulations. Furthermore, the present invention can produce flame-retardant hook-and-loop fasteners with selvages of a uniform width on both sides that are free of engaging elements and that run in a straight line in the warp direction without meandering. The present invention is also suitable for a method in which a wide hook-and-loop fastener, for example, 50 to 300 mm wide, is first produced and then slit in the warp direction to simultaneously produce multiple narrow hook-and-loop fasteners. In this case, in step A above, a loop woven fabric is woven in which, on the surface of the loop fabric, engaging element regions with engaging element loops and selvage regions without engaging element loops are each continuously present in the warp direction, and in the weft direction, the engaging element regions and selvage regions alternate, with multiple engaging element regions present. After step D above, the centers of the selvage regions are slit in the warp direction, thereby simultaneously producing multiple hook-and-loop fasteners with selvages of a uniform width on both sides. This method can also produce hook-and-loop fasteners in which the selvage regions run in a straight line in the warp direction without meandering. Of course, even in the case of a hook-and-loop fastener having a width of 15 mm or less, the present invention makes it difficult for the engaging elements to be pulled out of the base fabric even when repeated engagement and release are performed, and also produces a hook-and-loop fastener that hardly undulates in the vertical direction, has no meandering ears at both ends, and has no variation in the cut height of one leg of the hook-shaped engaging elements.
[0097] Furthermore, in the present invention, it is preferable to carry out the steps A through D continuously without winding up the woven fabric in between, since this makes it easier to obtain the effects of the present invention, further improving productivity, and also because it is easy to obtain hook-and-loop fasteners having engaging elements of the same hook or loop shape. In other words, with conventional woven fabric hook-and-loop fasteners, the process of applying a backcoat resin liquid to the back surface of the base fabric and drying the resin liquid takes time, so the woven fabric must be wound up once before applying the backcoat resin liquid and then wound up again once the resin liquid has dried, but this is not necessary with the present invention, and it can be said to be extremely superior in terms of productivity.
[0098] Furthermore, if winding is performed during the process, the loops for the engaging elements may collapse or be crushed in shape, or the loops for the engaging elements may be pressed down from above, causing the engaging elements to sink into the base fabric, which will have adverse effects even after passing through process D. However, in the present invention, the process can be run at the same speed from process A to process D, so there is no need to wind them in between, and therefore the adverse effects described above can be avoided. Furthermore, if winding is performed multiple times during production, losses will inevitably occur at the start and end of unwinding, reducing yield, but in the present invention, there is no intermediate winding, so there is less yield reduction.
[0099] The PPS woven hook-and-loop fastener thus obtained is a white hook-and-loop fastener with a slight brownish tint due to the influence of the PPS thread. Since this hook-and-loop fastener is often used in industrial applications where it is not visible to the human eye or where the color tone of the hook-and-loop fastener is not important, there is no need to dye it with dyes, pigments, or the like. However, if it is used in an application where it is visible to the human eye, it may be dyed with a disperse dye according to the user's request. Generally, PPS-based textile products are difficult to dye, so it is difficult to dye the hook-and-loop fastener of the present invention in dark colors. However, it is possible to obtain a product with a certain degree of dark color by dyeing it with a disperse dye using water as a medium at high temperature and high pressure.
[0100] When dyeing is performed using a disperse dye in water at high temperature and high pressure, the hook-and-loop fastener of the present invention can be dyed for 90 minutes or more in an aqueous solution containing the disperse dye at a temperature ranging from 120 to 145°C to obtain a PPS hook-and-loop fastener dyed to a relatively deep color. The type of disperse dye used is not particularly limited, and any disperse dye conventionally used for dyeing polyester fiber products can be used, including aminoazobenzene-based, anthraquinone-based, and nitroarylamine-based disperse dyes such as nitrodiphenylamine derivatives. Since PPS fiber products are used in heat-resistant and flame-retardant applications, black disperse dyes are preferred, as they can provide the color tone required for these applications.
[0101] The PPS woven hook-and-loop fastener obtained by the method described above is suitable for applications requiring high levels of flame retardancy and heat resistance, such as interior materials and seating materials for vehicles such as automobiles, airplanes, trains and ships, and attachment materials for curtains, and is particularly suitable as a fastening material for fastening the cushion and covering material of the seats of these vehicles, and also as a fastening material for floor carpets and curtain attachment materials for the above vehicles.It is also suitable for special clothing such as work clothes for use in high-temperature sites such as blast furnaces, foundries and glassware factories, and firefighting uniforms, and is also suitable as a fastening material in fields requiring flame retardancy and heat resistance, such as fastening materials for high-temperature gas filters.
[0102] The present invention will be described in detail below with reference to examples and comparative examples. In these examples and comparative examples, flame retardancy was measured in accordance with the vertical flame retardancy test method [14 CFR PART 25 Sec25.853(a)]. Specifically, the exposed surface of the hook-and-loop fastener was attached to a U-shaped jig in a combustion tester so that it was 5.08 cm x 30.48 cm long. The sample was then vertically placed and exposed to a flame from a hand burner from below for 12 seconds. The burning state was observed, and the time from when the burner was removed until the flame self-extinguished was measured. Five measurements were performed, and the average value was calculated.
[0103] The engaging force was measured in accordance with JIS L 3416-2000. When the surface fasteners of the Examples and Comparative Examples were hook surface fasteners, the mating loop surface fastener was B48000 (manufactured by Kuraray Fastening Co., Ltd.), and when the surface fasteners were loop surface fasteners, the mating hook surface fastener was A48600 (manufactured by Kuraray Fastening Co., Ltd.), and when the surface fasteners were hook-and-loop compatible surface fasteners, the same hook-and-loop compatible surface fastener was used as the mating surface fastener.
[0104] The pull-out force of the engaging elements was measured using a Shimadzu tensile tester. The hook-and-loop fastener was bent in the width direction (weft direction) to make it easier to grip the hook-shaped engaging elements and set in the chuck of the tensile tester. One hook-shaped engaging element of the set hook-and-loop fastener was gripped with pliers and pulled from the base fabric at a pulling speed of 100 mm / min. The maximum strength at which the hook-shaped engaging element was pulled out of the base fabric of the hook-and-loop fastener was measured. In the case of a loop hook-and-loop fastener, the loop-shaped engaging element thread that had sunk into the base fabric and then emerged to the surface was cut at the top of the base fabric surface, and the value measured in this state was measured using the above method. In the case of a hook-and-loop coexisting hook-and-loop fastener, the pull-out force of the hook-shaped engaging element was taken as the pull-out force of that engaging element. Ten hook-and-loop fasteners were randomly selected and their pull-out forces were measured, and the average value was used.
[0105] Example 1 The following yarns were prepared as warp yarns, weft yarns, and monofilament yarns for the hook-shaped engaging elements constituting the base fabric of a flame-retardant hook surface fastener. [Warp yarn] PPS multifilament yarn Total decitex and number of filaments: 250 dtex, 60 twists, 419 T / m Dry heat shrinkage at 200°C: 7.7%
[0106] [Weft yarn (untwisted parallel yarn of the following two types of multifilament yarn)] Multifilament yarn made of core-sheath composite filament Core component: polyethylene terephthalate Sheath component: polyethylene terephthalate copolymerized with 25 mol% isophthalic acid (softening point: 190°C) Core-sheath ratio (weight ratio): 70:30 Total decitex and number of filaments: 99 dtex, 24 filaments Dry heat shrinkage at 200°C: 17.1% Multifilament yarn made of PPS Total decitex and number of filaments: 167 dtex, 10 filaments Dry heat shrinkage at 200°C: 9.0%
[0107] [Monofilament thread for hook-shaped engaging element] PPS monofilament thread Diameter (before heat shrinkage): 0.20 mm Dry heat shrinkage at 200°C: 2.8%
[0108] [Manufacturing of Hook Surface Fasteners] Using the above warp yarns, weft yarns, and monofilament yarns for hook-shaped engaging elements, a plain weave was used to form loops on the base fabric, with a weave density (after heat shrinkage) of 56 warp yarns / cm and 16.5 weft yarns / cm, and the monofilament yarns for hook-shaped engaging elements were woven parallel to the warp yarns at a ratio of 1 for every 4 warp yarns, and after three weft yarns had floated and sunk, the monofilament yarns were made to straddle one warp yarn, forming a loop at the straddled point. When forming the loops for the hook-shaped engaging elements, metal rods having uniform longitudinal cross sections were placed parallel to the warp yarns at the position where the yarns for hook-shaped engaging elements straddled the warp yarns, with the same number of metal rods as the number of engaging element yarns aligned vertically so that the longitudinal direction of the cross sections was the height direction of the loops for hook-shaped engaging elements, and the yarns for engaging elements were made to straddle the tops of the metal rods, and after the loops were formed, the metal rods were pulled out of the loops.
[0109] The hook surface fastener tape woven under the above conditions was subjected to heat treatment by running it through a heat treatment oven for 60 seconds at 246°C, a temperature at which only the sheath component of the weft yarn was thermally melted but the warp yarns, the monofilament yarns for the hook-shaped engaging elements, and the core component of the weft yarn were not thermally melted, causing the warp yarns, the weft yarns, and the monofilament yarns for the hook-shaped engaging elements to thermally shrink. As a result, the tape shrunk by 8% in the weft direction, and the sheath component was melted, fusing the neighboring yarns.
[0110] While the heat-sealing component (sheath component) of the weft yarn remained molten, the fabric tape for hook surface fasteners was run along a fixed stainless steel surface with a mirror-finished surface installed immediately adjacent to the exit of the heat treatment furnace, as shown in Figure 1, with a tension of 200 g / cm applied after passing the fixed surface. The back side of the fabric was pressed against the fixed surface for 5 seconds, and the fabric was slid over the surface at a speed of 10 mm / sec for 5 seconds, and then the running direction was bent 90 degrees along the surface. The resulting fabric was then cooled, and one leg of the loop for the hook-like engaging element was cut to form the hook-like engaging element. As a result, no vertical waviness of the hook-like engaging element was observed, and therefore, the cutting of one leg of the hook-like engaging element was successfully carried out. Furthermore, the above-mentioned weaving process, heat treatment process, crimping process to the fixed surface, and cutting of one leg of the hook-like engaging element were carried out continuously without any intermediate winding steps.
[0111] [Performance of the Obtained Hook Surface Fastener] The width of the obtained hook surface fastener fabric was 20 mm in the region where the engaging elements were present, and at both ends thereof, selvages of 2.5 mm in width where no engaging elements were present were present in a uniform width parallel to the warp direction without meandering. When the flame retardancy of this hook surface fastener was measured, it was found to be extremely excellent at 3.4 seconds, which was a level that was fully acceptable for aircraft applications.
[0112] In this hook surface fastener, the density of the hook-shaped engaging elements is 56 pieces / cm 2The height of the hook-shaped engaging elements from the surface of the base fabric was 1.8 mm. When the broken state of the hook-shaped engaging elements of the hook-and-loop fastener was observed, it was found that all of the hook-shaped engaging elements were broken at a point 70% of the height from the base of one leg. Furthermore, when the warp thickness (Tb) in the thickness direction of the base fabric at the point where this hook-and-loop fastener was most deeply sunk on the back side and the warp thickness (Ts) in the thickness direction of the base fabric at the point where it was most raised on the front side were measured, (Tb) was 0.125 mm and (Ts) was 0.107 mm, so that (Tb) / (Ts) was 0.86.
[0113] The pull-out force of the hook-shaped engaging elements of this hook surface fastener from the base fabric was measured and found to be 6.3 N, indicating that it also has excellent pull-out resistance. Furthermore, the presence or absence of vertical waviness of this surface fastener was observed by placing the surface fastener on a flat glass plate without applying any load, and no waviness was observed at all.
[0114] Furthermore, when the engagement strength of this hook surface fastener was measured, the initial engagement strength was 12.4 N / cm in shear strength. 2 , peel strength is 1.39 N / cm, engagement force after 1000 engagement / peel cycles is shear strength of 11.2 N / cm 2 The peel strength was 1.26 N / cm, and even after 1000 repeated engagement and peeling cycles, no hook-shaped engaging elements were found to have been pulled out from the surface of the hook surface fastener or any hook-shaped engaging elements that had become so stretched that they had lost their ability to engage. This showed that the hook surface fastener was extremely excellent, despite the absence of a backcoat layer.
[0115] Furthermore, because this hook-and-loop fastener is flexible, it can be attached to the cuffs of clothing by sewing its selvage with a sewing machine without compromising the appearance of the clothing. In this case, the sewing thread can be sewn in a straight line through the center of the selvage without meandering around the selvage, resulting in an excellent appearance.
[0116] Comparative Example 1 [Manufacturing of Hook Surface Fastener] A hook surface fastener was manufactured in the same manner as in Example 1, except that the stainless steel fixed surface installed immediately adjacent to the outlet of the heat treatment furnace was removed, and instead of pressing the back side of the surface of the surface fastener against the fixed surface while the heat-fusible multifilament yarn was still in a molten state after heat treatment, the surface was removed from the heat treatment furnace, cooled, and then pulled up with a roller.
[0117] [Performance of the obtained hook surface fastener] The obtained hook surface fastener had an area with engaging elements that was 20 mm wide, and at both ends thereof, ears with an average width of 2.5 mm and no engaging elements were present, which were parallel to the warp direction. The density of the hook-shaped engaging elements of this hook surface fastener was 56 pieces / cm 2 The height of the hook-shaped engaging elements from the surface of the base fabric was 1.8 mm, and the flame retardancy was 3.6 seconds, which was as excellent as that of Example 1. When the cut state of the hook-shaped engaging elements was observed, it was found that some were cut near the base of the hook-shaped engaging elements, and some were cut near the top, and some were loop-like with one leg not cut at the base, some had both legs cut and were not hook-shaped, and some were only cut halfway down one leg. When this hook-and-loop fastener was placed on a horizontal glass plate, large and small waviness in the vertical direction was observed, and areas that had lifted off the glass plate were repeatedly observed.
[0118] The pull-out force of the hook-shaped engaging elements of this hook surface fastener was measured to be 4.2 N, a result considerably inferior to that of Example 1. Furthermore, when the engaging force of this hook surface fastener was measured, the initial engaging force was 11.6 N / cm in shear strength. 2 , peel strength is 1.28 N / cm, engagement force after 1000 engagement / peel cycles is shear strength of 9.7 N / cm 2 The peel strength was 1.02 N / cm, and after 1000 repeated engagement and peeling cycles, hook-shaped engaging elements were occasionally found pulled out from the surface of the hook surface fastener.
[0119] The (Tb) / (Ts) ratio of this hook surface fastener was 0.96. Furthermore, when this hook surface fastener was attached to the cuff of a garment by sewing with a sewing thread using the selvage, as in Example 1, it was difficult to sew the center with the sewing thread due to the meandering of the selvage, and the surface fastener on the sewn cuff had meandering sewing thread in places and was inferior to that of Example 1 in terms of appearance.
[0120] Example 2 [Manufacturing of Loop Hook Fastener] A loop hook fastener was manufactured in the same manner as in Example 1, except that the yarn for the engaging elements was changed to the multifilament yarn for the loop-shaped engaging elements described below, a plain weave was used as the weave, and the weave density (after heat shrinkage treatment) was 54 warp threads / cm and 18.8 weft threads / cm. The multifilament yarn for the loop-shaped engaging elements was woven parallel to the warp threads at a ratio of 1 for every 4 warp threads, and a loop was formed on the base fabric at the location where it was straddled after three weft threads were floated and sunk. Because the engaging elements were loop-shaped engaging elements, cutting one leg of the loop in step D, which was performed in Example 1, was not performed. Furthermore, the above-mentioned weaving process, heat treatment process, and crimping process to the fixed surface were performed continuously without any winding in between. [Thread for loop-shaped engaging element] Multifilament thread made of PPS Total decitex and number of filaments: 334 dtex and 20 filaments Dry heat shrinkage at 200°C: 9.1%
[0121] [Performance of the obtained loop surface fastener] The width of the obtained woven fabric for loop surface fastener was 20 mm in the area where the engaging elements were present, and at both ends of the fabric there were 2.5 mm wide ears where no loop engaging elements were present and were of uniform width parallel to the warp direction. The flame retardancy of this loop surface fastener was measured and found to be extremely excellent at 3.0 seconds, which was found to be at a level that could pass for aircraft applications like that of Example 1, and it was found that it could be used in combination with that of Example 1.
[0122] The density of the loop engaging elements of this loop surface fastener is 63 pieces / cm 2The height of the loop engaging elements from the surface of the base fabric was 2.1 mm. The (Tb) / (Ts) ratio of this loop surface fastener was 0.88. Next, the pull-out force of this loop engaging element was measured and found to be 10.3 N, indicating that it also had excellent pull-out resistance. Furthermore, the loop surface fastener was placed on a flat glass plate and observed for vertical waviness, and no waviness was observed at all.
[0123] Furthermore, when the engagement strength of this loop hook-and-loop fastener was measured, the initial engagement strength was 12.2 N / cm in shear strength. 2 , peel strength is 1.38 N / cm, engagement force after 1000 engagement / peel cycles is shear strength of 11.1 N / cm 2 The hook surface fastener had a peel strength of 1.24 N / cm, and even after 1000 repeated engagement and peeling cycles, no loop engaging elements were found to have been pulled out from the surface of the loop surface fastener, demonstrating that the loop surface fastener has an extremely excellent engaging strength despite the absence of a backcoat layer. Furthermore, because this hook surface fastener is extremely flexible, when it was attached to the cuff of a garment by sewing with a sewing thread using the selvage, the sewing thread did not snake around the selvage but ran in a straight line through the center of the selvage, giving it an excellent appearance.
[0124] Comparative Example 2 [Manufacturing of Loop Hook and Loop Fastener] A loop hook and loop fastener was manufactured in the same manner as in Example 2, except that the stainless steel fixed surface installed immediately next to the outlet of the heat treatment furnace was removed, and the back side of the hook and loop fastener was not pressed against the fixed surface while the heat-fusible multifilament yarn remained in a molten state after heat treatment, and the hook and loop fastener was cooled and then pulled up with a roller.
[0125] [Performance of the obtained loop surface fastener] The obtained loop surface fastener had an area with engaging elements that was 20 mm wide, and at both ends thereof, ears with an average width of 2.5 mm and no engaging elements were present, which were parallel to the warp direction. The density of the loop engaging elements of this loop surface fastener was 63 pieces / cm 2The height of the loop-shaped engaging elements from the surface of the base fabric was 2.1 mm, and the flame retardancy was 3.1 seconds. When this hook and loop fastener was placed on a horizontal glass plate, large and small waviness in the vertical direction was observed, similar to the hook and loop fastener of Comparative Example 1.
[0126] Furthermore, the pull-out force of the loop-shaped engaging element from the surface of the base fabric was measured, and the result was 8.7 N, which was inferior to that of Example 2. Furthermore, when the engaging force of this loop surface fastener was measured, the initial engaging force was 11.4 N / cm in shear strength. 2 , peel strength is 1.26 N / cm, engagement force after 1000 engagement / peel cycles is shear strength of 9.6 N / cm 2 The peel strength was 1.01 N / cm, and the engagement strength was inferior to that of Example 2. Furthermore, after 1000 repeated engagement and peeling cycles, loop-shaped engagement elements were seen in some places being pulled out from the surface of the loop surface fastener, unlike that of Example 2.
[0127] The (Tb) / (Ts) ratio of this loop hook-and-loop fastener was 0.97. This loop hook-and-loop fastener was attached to the cuff of a garment by sewing with a sewing thread using its ears, as in Example 2. However, it was difficult to sew the center of the ears with the sewing thread, and as a result, the sewing thread appeared to meander slightly, and the appearance was inferior to that of Example 2.
[0128] Example 3 [Production of a hook-and-loop co-existing surface fastener] A hook-and-loop co-existing surface fastener was produced using the warp yarns, weft yarns, monofilament yarns for hook-shaped engaging elements, and multifilament yarns for loop-shaped engaging elements used in Examples 1 and 2. Specifically, a plain weave was used as the weave structure, with a weave density (after heat shrinkage treatment) of 54 warp yarns / cm and 16.5 weft yarns / cm, and a multifilament yarn for loop-shaped engaging elements or a monofilament yarn for hook-shaped engaging elements was used at a ratio of one for every four warp yarns, and loops were formed on the base fabric so that three weft yarns were floated and sunk and then straddled one warp yarn, forming a loop at the straddled point. In this process, the multifilament yarns for loop-shaped engaging elements and the monofilament yarns for hook-shaped engaging elements were woven in such a way that they were continuously alternated in units of two.
[0129] A hook-and-loop coexisting surface fastener was manufactured by weaving the fabric in the same manner as in Example 1, heat-treating the fabric, pressing the fabric against a fixed surface, and cutting one leg of the loop for the hook-like engaging element in the same manner as in Example 1. The above-mentioned weaving, heat-treating, pressing the fabric against a fixed surface, and cutting one leg of the hook-like engaging element were all carried out continuously without any winding in between.
[0130] [Performance of the obtained hook-and-loop coexisting surface fastener] The width of the obtained woven fabric for a hook-and-loop coexisting surface fastener was 20 mm in the region where the engaging elements were present, and 2.5 mm wide selvedge portions where no engaging elements were present were present at both ends of the woven fabric in a uniform width parallel to the warp direction. The density of the hook-shaped engaging elements was 28 pieces / cm 2 , the density of the loop-shaped engaging elements is 28 pieces / cm 2 Furthermore, the height of the hook-shaped engaging elements from the surface of the base fabric was 1.8 mm, and the height of the loop-shaped engaging elements from the surface of the base fabric was 2.1 mm. The flame retardancy of this hook-and-loop compatible surface fastener was 3.2 seconds, which was found to be at a level suitable for use in aircraft applications, similar to those of Examples 1 and 2.
[0131] When the state of breakage of the hook-like engaging elements of this hook-and-loop concurrent type surface fastener was observed, it was found that all of the hook-like engaging elements had been broken at a location that was 70% of the height from the base of one leg. The (Tb) / (Ts) ratio of this hook-and-loop concurrent type surface fastener was 0.87.
[0132] Next, the pull-out forces of the hook-shaped engaging elements and the loop-shaped engaging elements were measured and found to be 6.5 N and 9.9 N, respectively, demonstrating that they also have extremely excellent pull-out resistance. Furthermore, the presence or absence of vertical waviness of this hook-and-loop fastener was observed by placing the hook-and-loop fastener on a flat glass plate in the same manner as in Examples 1 and 2, and no waviness was observed at all.
[0133] Furthermore, when the engagement strength of this hook-and-loop surface fastener was measured, the initial engagement strength was 10.1 N / cm in shear strength. 2, peel strength is 1.02 N / cm, engagement force after 1000 engagement / peel cycles is shear strength of 9.6 N / cm 2 The results showed that the hook-and-loop compatible surface fastener had a peel strength of 0.97 N / cm, which is an extremely excellent value for a hook-and-loop compatible surface fastener. Even after 1,000 repeated engagement and peeling cycles, no engaging elements were found to be pulled out from the surface of the hook-and-loop compatible surface fastener, demonstrating that the hook-and-loop compatible surface fastener is extremely excellent, despite the absence of a backcoat layer. Because this hook-and-loop compatible surface fastener is extremely flexible, when its selvage is used to sew it to the cuff of a garment, the sewing thread can be sewn in a straight line through the center of the selvage without meandering, and the appearance is also excellent.
[0134] Comparative Example 3 [Production of a hook-and-loop coexisting surface fastener] A hook-and-loop coexisting surface fastener was produced in the same manner as in Example 3, except that the fixing surface attached immediately adjacent to the outlet of the heat treatment furnace was removed and the process of pressing the back side of the hook-and-loop fastener against this fixing surface while the heat-fusible multifilament yarn was still in a molten state after the heat treatment was omitted, and the hook-and-loop fastener removed from the heat treatment furnace was cooled and then pulled up with rollers.
[0135] [Performance of the obtained hook-and-loop coexisting surface fastener] The obtained hook-and-loop coexisting surface fastener had a region with engaging elements that was 20 mm wide, and at both ends thereof, ears with an average width of 2.5 mm and no engaging elements were present, which were parallel to the warp direction. The density of the hook-like engaging elements of this hook-and-loop coexisting surface fastener was 28 pieces / cm 2 , the density of the loop-shaped engaging elements is 28 pieces / cm 2 Furthermore, the height of the hook-shaped engaging elements from the surface of the base fabric was 1.8 mm, and the height of the loop-shaped engaging elements from the surface of the base fabric was 2.1 mm. The flame retardancy of this hook-and-loop combined surface fastener was excellent at 3.4 seconds.
[0136] When the state of breakage of the hook-shaped engaging elements of this hook-and-loop coexisting surface fastener was observed, a small number of breakages were observed, such as those near the base or almost at the top, similar to that of Comparative Example 1. Next, when this surface fastener was placed on a horizontal glass plate and the state of waviness was observed, large waviness in the vertical direction was frequently observed, with fine waviness within that, similar to the hook surface fasteners of Comparative Example 1 and the loop surface fasteners of Comparative Example 2.
[0137] Furthermore, the pull-out forces of the hook-shaped engaging elements and the loop-shaped engaging elements were measured and found to be 4.1 N and 8.6 N, respectively, both of which were inferior to those of Example 3. Furthermore, when the engaging force of this hook-and-loop combined surface fastener was measured, the initial engaging force was 9.2 N / cm in shear strength. 2 , peel strength is 0.92 N / cm, engagement force after 1000 engagement / peel cycles is shear strength of 8.1 N / cm 2 The peel strength was 0.80 N / cm, and after 1000 repeated engagement and peeling cycles, a small number of hook-shaped engaging elements were observed to be pulled out from the surface of the hook-and-loop coexisting surface fastener.
[0138] The (Tb) / (Ts) ratio of this hook and loop compatible surface fastener was 0.97. This hook and loop compatible surface fastener was sewn to the cuff of a garment using a sewing thread, using its ears, in the same way as the surface fastener of Example 3. However, it was difficult to sew the center of the ears with the sewing thread, and as a result, the sewing thread appeared to meander, and the appearance was inferior to that of Example 3.
[0139] Example 4 [Production of Hook Surface Fastener] A hook surface fastener was produced in the same manner as in Example 1, except that the fixed surface against which the heat-fusible core-sheath filaments were pressed while they were still in a molten state was replaced with a stainless steel mirror-finished roll surface with a matte surface. The roll surface rotated 5 mm / sec slower than the running speed of the hook surface fastener fabric, which ran in contact with it. The contact time between the back surface of the base fabric and the roll surface was 5 seconds. The heat-fusible fibers were pressed against the roll surface while still in a molten state and slid across the roll surface. A tension of 250 g / cm was applied to the base fabric after passing through the roll surface. The above-mentioned weaving process, heat treatment process, pressing process onto the roll surface, and even the process of cutting one leg of the hook-shaped engaging element were all carried out continuously without any winding in between.
[0140] [Performance of the Obtained Hook Surface Fastener] The width of the obtained hook surface fastener fabric was 20 mm in the region where the engaging elements were present, and at both ends of the fabric were 2.5 mm wide ears where no engaging elements were present, with a uniform width parallel to the warp direction. The hook-like engaging element density and the height of the hook-like engaging elements from the surface of the base fabric of this hook surface fastener were the same as those of Example 1. The flame retardancy of this hook surface fastener was 3.5 seconds, which was extremely excellent, just like that of Example 1. The (Tb) / (Ts) ratio of this hook surface fastener was 0.92.
[0141] Furthermore, the pull-out force of the hook-shaped engaging elements of this hook surface fastener was 6.0 N, demonstrating excellent pull-out resistance. Furthermore, when the hook-and-loop fastener was placed on a flat glass plate to check for vertical waviness, almost no significant waviness was observed, but some areas were slightly raised above the glass surface. Regarding the cut state of the hook-shaped engaging elements, all of the hook-shaped engaging elements were cut at a point that was approximately 70% of the height of one leg, but in some cases the cut point was slightly misaligned in the vertical direction.
[0142] Furthermore, when the engagement strength of this hook surface fastener was measured, the initial engagement strength was 12.0 N / cm in shear strength. 2, peel strength is 1.35 N / cm, engagement force after 1000 engagement / peel cycles is shear strength of 10.9 N / cm 2 The peel strength was 1.21 N / cm, which was an excellent value. Even after 1,000 repeated engagement and peeling cycles, almost no hook-shaped engaging elements were found to have been pulled out from the surface of the hook surface fastener. When the ears of this hook surface fastener were used to sew the cuffs of clothing with a sewing thread, the sewing thread was able to sew in an almost straight line through the center of the ears without meandering, although some parts were found to be slightly off-center.
[0143] Example 5 [Production of Loop Hook and Loop Fastener] A loop hook and loop fastener was produced in the same manner as in Example 2, except that the fixed surface against which the heat-fusible sheath-core filaments were pressed while they were kept in a molten state was replaced with a stainless steel roll surface having a matte surface, as in Example 4. The rotation speed and tension of the roll surface were the same as in Example 2.
[0144] [Performance of the obtained loop surface fastener] The width of the obtained loop surface fastener fabric and the width of the selvage were the same as in Example 2, and the selvages were uniformly spaced parallel to the warp direction. The density of the loop engaging elements and the height of the loop engaging elements from the surface of the base fabric of this loop surface fastener were the same as in Example 2. The flame retardancy of this loop surface fastener was 3.3 seconds, which was extremely excellent. The (Tb) / (Ts) ratio of this loop surface fastener was 0.93.
[0145] Furthermore, the pull-out force of the loop-shaped engaging elements of this loop surface fastener was 9.6 N, and it was found to have excellent pull-out resistance. Furthermore, when this surface fastener was placed on a flat glass plate to check whether or not there was any waviness in the vertical direction, almost no significant waviness was observed, but similar to the surface fastener of Example 4 above, some areas were observed to be slightly raised from the glass surface.
[0146] Furthermore, when the engagement strength of this loop hook-and-loop fastener was measured, the initial engagement strength was 11.8 N / cm in shear strength. 2, peel strength is 1.31 N / cm, engagement force after 1000 engagement / peel cycles is shear strength of 10.5 N / cm 2 The peel strength was 1.17 N / cm, which was an excellent value. When the ears of this loop hook-and-loop fastener were used to sew to the cuffs of a garment with a sewing thread, the sewing thread was able to sew in a straight line through the center of the ears with almost no meandering, but as in the case of Example 4 above, some of the threads were not centered, and the appearance was slightly inferior to that of Example 2.
[0147] Comparative Example 4 [Production of Hook Surface Fastener] A hook surface fastener was produced in the same manner as in Example 1, except that instead of using a combined yarn of polyphenylene sulfide multifilament yarn and a multifilament yarn made of a heat-fusible filament in Example 1, a yarn consisting solely of a multifilament yarn made of a core-sheath type composite filament was used as the weft yarn. [Weft yarn (multifilament yarn made of core-sheath type composite filament)] The core component, sheath component, and core-sheath ratio were the same as those used for the weft yarn in Example 1. Total decitex and number of filaments: 240 dtex and 48 filaments. Dry heat shrinkage at 200°C: 17.0%
[0148] [Performance of the obtained hook surface fastener] The obtained hook surface fastener had no problems with vertical waviness, pull-out resistance of the engaging elements, engaging force, etc., but its flame retardancy was 19.2 seconds, which was far inferior to that of Example 1 and was not flame retardant enough for use in aircraft applications.
[0149] Example 6 [Production of Hook Surface Fasteners] The same procedure as in Example 1 was used, except that the PPS multifilament yarn used as the weft yarn for the paralleled yarn consisting of a PPS multifilament yarn and a multifilament yarn made of a heat-fusible filament was replaced with the following PPS multifilament yarn. A wide hook surface fastener was produced, with four 20 mm wide regions where engaging elements are present, arranged parallel to the warp direction, and at one end of each region, three 2.5 mm wide ear regions and three 5 mm wide middle ear regions sandwiched between the engaging element regions, arranged parallel to the warp direction, with the engaging element regions and middle ear regions alternating in the weft direction. Finally, the center of the middle ear region was slit parallel to the warp direction to produce four hook surface fasteners. The remaining production conditions were the same as in Example 1. [Multifilament yarn made of PPS used as the paralleled weft yarn] Total decitex and number of filaments: 250 dtex, 60 filaments Dry heat shrinkage at 200°C: 7.8%
[0150] [Performance of the Obtained Hook Surface Fasteners, etc.] The density of the hook-like engaging elements and the height of the hook-like engaging elements from the surface of the base fabric for the four obtained hook surface fasteners were almost the same as those for Example 1, and with regard to the cut state of the hook-like engaging elements of the surface fasteners, all of the hook-like engaging elements were cut at a location that was almost 70% of the height of one leg. The flame retardancy of this hook surface fastener was measured and found to be 2.0 seconds, which was extremely excellent, similar to that of Example 1. The (Tb) / (Ts) ratio of this hook surface fastener was 0.87.
[0151] The pull-out force of the hook-shaped engaging elements of this hook surface fastener was 6.1 N, and although slightly inferior to that of Example 1, its pull-out resistance was still extremely excellent. Furthermore, no vertical waviness was observed on this surface fastener, as with Example 1, and the center of the middle ear region was precisely slit, with the resulting ears having a consistent width of 2.5 mm. This surface fastener was cut into 15 cm lengths and washed 50 times, but no fraying was observed at the edges of the slit ears.
[0152] Furthermore, when the engagement strength of this hook surface fastener was measured, the initial engagement strength was 12.2 N / cm in shear strength. 2 , peel strength is 1.36 N / cm, engagement force after 1000 engagement / peel cycles is shear strength of 11.1 N / cm 2 The peel strength was 1.24 N / cm, which was an extremely excellent value. Even after 1000 repeated engagement and peeling cycles, there were almost no hook-shaped engaging elements that had been pulled out from the surface of the hook surface fastener or hook-shaped engaging elements that had fully stretched out. When the ears of this hook surface fastener were used to sew the cuffs of clothing with a sewing thread, the sewing thread could easily sew in a straight line through the center of the ears.
[0153] Comparative Example 5 [Manufacturing of Hook Surface Fasteners] Four hook surface fasteners were produced in the same manner as in Example 6, except that the fixed stainless steel surface installed immediately adjacent to the outlet of the heat treatment furnace was removed, and instead of pressing the back side of the surface fastener while the heat-fusible multifilament yarn was still in a molten state after heat treatment, the surface fastener was cooled and then pulled up with a roller.
[0154] [Performance of the Obtained Hook Hook Fasteners] The obtained hook hook fasteners all had a 20 mm wide engaging element region, similar to Example 6, with ears at both ends having an average width of 2.5 mm parallel to the warp direction. When the cut state of the hook-shaped engaging elements of these hook hook fasteners was observed, it was found to be similar to that of Comparative Example 1. The vertical waviness of these hook fasteners was also similar to that of Comparative Example 1, with both large and small waviness observed, and areas that had lifted from the glass plate repeatedly observed. Due to the waviness, it was difficult to accurately slit the center of the middle ear region to a width of 2.5 mm, and wide and narrow areas were observed in many places. Furthermore, when these hook fasteners were cut to lengths of 15 cm and repeatedly washed 50 times, it was observed that approximately 20% of the hook fasteners had warp fraying from the ends of the slit ears.
[0155] The pull-out force and engagement force of the hook-shaped engaging elements of this hook surface fastener were almost the same as those of Comparative Example 1, and the number of hook-shaped engaging elements pulled out from the surface after 1,000 repeated engagement and peeling cycles was also the same as that of Comparative Example 1. The (Tb) / (Ts) ratio of this hook surface fastener was 0.96, the same as that of Comparative Example 1. Furthermore, when this hook surface fastener was attached to the cuff of a garment using the ears with a sewing machine, it was difficult to sew the center with a sewing thread due to the uneven width and meandering of the ears.
[0156] Example 7 [Production of Loop Hook and Loop Fastener] The same procedures as in Example 2 were carried out except that the PPS multifilament yarn used as the weft yarn for the paralleled yarn consisting of a PPS multifilament yarn and a multifilament yarn made of a heat-fusible filament was replaced with the same PPS multifilament yarn as used in Example 6, and a loop hook and loop fastener in which 20 mm-wide engaging element regions and 5 mm-wide ear regions were alternately arranged in the weft direction was produced in the same manner as in Example 6. Finally, four loop hook and loop fasteners were produced by slitting the centers of the ear regions parallel to the warp direction. The other production conditions were the same as in Example 2 except that the tension after passing through the fixed surface was changed from 200 g / cm to 400 g / cm.
[0157] [Performance of the obtained loop surface fastener, etc.] The density and height from the base fabric surface of the loop engaging elements for the four obtained loop surface fasteners were almost the same as those of Example 2. When the flame retardancy of this loop surface fastener was measured, it was 3.3 seconds, which was extremely excellent, similar to that of Example 2. In addition, the (Tb) / (Ts) ratio of this loop surface fastener was 0.82.
[0158] The pull-out force of the loop-shaped engaging elements of this loop surface fastener was 9.8 N, and it also had extremely excellent pull-out resistance. Furthermore, as with Example 2, no vertical waviness was observed on this surface fastener, and the ears generated from the middle ear region by the slits were 2.5 mm wide and existed in a straight line parallel to the warp direction. Furthermore, when this surface fastener was cut into 15 cm lengths and repeatedly washed 50 times, no fraying of the warp yarns from the slit ears was observed, as with the hook surface fastener of Example 6.
[0159] Furthermore, when the engagement strength of this loop hook-and-loop fastener was measured, the initial engagement strength was 12.0 N / cm in shear strength. 2 , peel strength is 1.34 N / cm, engagement force after 1000 engagement / peel cycles is shear strength of 10.8 N / cm 2 The peel strength was 1.21 N / cm, which was an extremely excellent value. Even after 1000 repeated engagement and peeling cycles, no loop engaging elements were found to have been pulled out from the surface of the loop surface fastener. When the ears of this loop surface fastener were used to sew the cuffs of clothing with a sewing thread, the sewing thread was able to sew in a straight line through the center of the ears, and the appearance was also excellent.
[0160] Comparative Example 6 [Manufacturing of Loop Hook and Loop Fasteners] Four loop hook and loop fasteners were manufactured in the same manner as in Example 7, except that the fixed stainless steel surface installed immediately next to the outlet of the heat treatment furnace was removed, and the back side of the hook and loop fastener was cooled without being pressed while the heat-fusible multifilament yarn remained molten after the heat treatment, and then pulled up with a roller.
[0161] [Performance of the obtained loop surface fasteners, etc.] The obtained loop surface fasteners all had an engaging element region with a width of 20 mm, and had ears with an average width of 2.5 mm at both ends parallel to the warp direction, similar to Example 7. The loop surface fasteners showed both large and small waviness in the vertical direction, similar to that of Comparative Example 2. The slit ears made it difficult to accurately slit the center of the middle ear region due to the waviness, and wide and narrow areas were frequently observed.
[0162] The pull-out force and engagement force of the loop-shaped engaging elements of this loop surface fastener were almost the same as those of Comparative Example 2. The (Tb) / (Ts) ratio of this hook surface fastener was 0.97, the same as that of Comparative Example 2. Furthermore, when this loop surface fastener was attached to the cuff of a garment using its ears with a sewing machine, it was difficult to sew the center with a sewing thread due to the uneven width and meandering of the ears.
[0163] Example 8 [Production of Hook Surface Fastener] A hook surface fastener was produced under the same conditions as in Example 1 above, except that the tension after passing through the fixed surface was changed from 200 g / cm to 640 g / cm.
[0164] [Performance of the Obtained Hook Surface Fastener] The density of the hook-like engaging elements and the height of the hook-like engaging elements from the surface of the base fabric for the obtained hook surface fastener were exactly the same as those in Example 1, and the cut state of the hook-like engaging elements of the surface fastener was also extremely uniform, being the same as that in Example 1. Furthermore, the flame retardancy was also extremely excellent, being the same as that in Example 1. The warp thickness (Tb) in the thickness direction of the base fabric at the point where this hook surface fastener was most sunken on the back side and the warp thickness (Ts) in the thickness direction of the base fabric at the point where it was most raised on the front side were measured, and the ratio (Tb) / (Ts) was 0.76.
[0165] The pull-out force of the hook-shaped engaging elements of this hook surface fastener was 6.2 N, and the pull-out resistance was also extremely excellent, similar to that of Example 1. Furthermore, no vertical waviness of this surface fastener was observed, similar to that of Example 1. When the engaging force of this hook surface fastener was measured, the initial engaging force was 12.2 N / cm in shear strength. 2 , peel strength is 1.36 N / cm, engagement force after 1000 engagement / peel cycles is shear strength of 11.1 N / cm 2 The peel strength was 1.24 N / cm, which was an extremely excellent value. Even after 1000 repeated engagement and peeling cycles, no hook-shaped engaging elements were found to have been pulled out from the surface of the hook surface fastener or to have been fully stretched.
[0166] When the ears of this hook fastener were used to sew onto the cuffs of clothing with a sewing thread, the sewing thread was able to sew in a straight line through the center of the ears. However, since the base fabric of this hook fastener was more rigid than that of Example 1, it was somewhat less easy to attach to fabric, and furthermore, due to this rigidity, it was not necessarily suitable for use on clothing or other items that come into contact with the human body.
[0167] Example 9 [Production of Loop Hook and Loop Fastener] A loop hook and loop fastener was produced under the same conditions as in Example 2 above, except that the tension after passing through the fixed surface was changed from 200 g / cm to 560 g / cm.
[0168] [Performance of the obtained loop surface fastener] The density of the loop engaging elements and the height of the loop engaging elements from the surface of the base fabric of the obtained loop surface fastener were exactly the same as those of Example 2. Furthermore, the flame retardancy was also extremely excellent, the same as that of Example 2. The (Tb) / (Ts) ratio of this loop surface fastener was 0.74.
[0169] The pull-out force of the loop-shaped engaging element of this loop surface fastener was 10.2 N, and the pull-out resistance was also extremely excellent, similar to that of Example 2. Furthermore, no vertical waviness of this surface fastener was observed, similar to that of Example 2. When the engaging force of this loop surface fastener was measured, the initial engaging force was 12.0 N / cm in shear strength. 2 , peel strength is 1.34 N / cm, engagement force after 1000 engagement / peel cycles is shear strength of 10.7 N / cm 2 The peel strength was 1.20 N / cm, which was an extremely excellent value. Even after 1000 repeated engagement and peeling cycles, no loop engaging elements were found to have been pulled out from the surface of the loop surface fastener.
[0170] When the ears of this loop hook-and-loop fastener were used to sew to the cuffs of clothing with a sewing thread, the sewing thread was found to be in a straight line at the center of the ears. However, since the base fabric of this hook-and-loop fastener was slightly more rigid than that of Example 2, it could not be said to be optimal for applications where it would come into contact with the human body, just like the hook-and-loop fastener of Example 8.
[0171] Comparative Example 7 [Production of Hook Hook Fastener] In Example 1 above, a fixed stainless steel surface with a mirror-finished surface that had been installed immediately adjacent to the exit of the heat treatment furnace was moved 85 cm from the exit, and the backside of the fixed surface was heated so that the surface temperature of the fixed surface reached 160° C. A hook hook fastener was produced in the same manner as in Example 1, except that the heat-treated fabric tape for a hook hook fastener of Example 1 above was pulled out from the exit of the heat treatment furnace and allowed to run for 85 cm (the tape was naturally cooled during running, and it was confirmed that the heat-fusible component used in the weft yarn had sufficiently solidified), the backside of the cooled tape was pressed against the fixed surface whose surface temperature was 160° C. for 5 seconds, and slid across the same surface, and then the running direction of the tape was bent 90 degrees along the same surface, and after passing the fixed surface, it was taken up under a tension of 200 g / cm.
[0172] [Performance of the Obtained Hook Surface Fastener] The obtained hook surface fastener was similar in performance to that of Comparative Example 1, i.e., it had excellent flame retardancy equivalent to that of Example 1, but when placed on a horizontal glass plate, large and small waviness in the vertical direction was observed, and furthermore, some hook-shaped engaging elements had the base of one leg uncut and remained in a loop shape, some had both legs cut, and some had only one leg cut partway down were observed in some places. The hook-shaped engaging element density was 56 pieces / cm 2 The height of the hook-shaped engaging element from the surface of the base fabric was 1.8 mm. A few consecutive instances of one leg of the hook-shaped engaging element being cut off, such as at a position near the base of the hook-shaped engaging element or at a position near the top, were observed.
[0173] The pull-out force of the hook-shaped engaging element was 4.4 N, which was considerably inferior to that of Example 1. Furthermore, when the engaging force of this hook surface fastener was measured, the initial engaging force was 11.8 N / cm in shear strength. 2 , peel strength is 1.29 N / cm, engagement force after 1000 engagement / peel cycles is shear strength of 9.9 N / cm 2 The peel strength was 1.04 N / cm, and after 1000 repeated engagement and peeling cycles, hook-shaped engaging elements were occasionally found pulled out from the surface of the hook surface fastener.
[0174] The (Tb) / (Ts) ratio of this hook surface fastener was 0.96. When this hook surface fastener was attached to fabric using a sewing thread at the selvage, it was difficult to sew the center of the selvage with the sewing thread, and as a result, the sewing thread appeared to meander, and the appearance was inferior to that of Example 1.
[0175] Comparative Example 8 [Production of Hook Hook Fastener] The hook hook fastener produced in Comparative Example 1 above was wound around a smooth-surfaced stainless steel heated roll with a diameter of 12.5 cm, with the engaging element side facing outward, without being pressed against the roll, and in this state was subjected to a heat treatment at 195°C for 20 minutes. In order to minimize the possibility of the engaging elements being knocked over by the pressure during winding, the lower layer hook fastener was wound so as not to be pressed down by the upper layer hook fastener, that is, a winding method was used that minimized tightening. After this heat treatment was completed, the hook fastener was cooled and removed from the heated roll, and the performance of the heat-treated hook hook fastener and the state of the hook-shaped engaging elements were observed and measured.
[0176] [Performance of the obtained hook surface fastener] As a result, at first glance it appeared to be almost the same as that of Comparative Example 1, but when this surface fastener was placed on a horizontal glass plate, large and small waviness in the vertical direction was observed, it did not adhere to the glass plate, and the effect of eliminating the waviness by the above heat treatment was not obtained at all.
[0177] Measurement of the pull-out force of the hook-shaped engaging elements of this hook surface fastener revealed a value of 4.1 N, which was approximately the same as that of Comparative Example 1. Furthermore, when the engaging force of this hook surface fastener was measured, the initial engaging force and the engaging force after 1000 engagements and peelings were also approximately the same as those of Comparative Example 1, and after 1000 engagements and peelings, hook-shaped engaging elements were occasionally found pulled out from the surface of the hook surface fastener.
[0178] The (Tb) / (Ts) ratio of this hook surface fastener was also 0.96, unchanged from that of Comparative Example 1. Furthermore, when this hook surface fastener was attached to the cuff of a garment by sewing with a sewing thread using the ear portion, it was difficult to sew the center of the ear portion with the sewing thread, and the sewing thread of the surface fastener on the sewn cuff had meandering in places.
[0179] Comparative Example 9 [Production of Hook Surface Fastener] A hook surface fastener was produced in the same manner as in Example 4, except that the surface speed of the roll surface was the same as the running speed of the hook surface fastener fabric, and the back surface of the fabric was pressed onto the roll surface but was not sliding on the roll surface.
[0180] [Performance of the Obtained Hook Surface Fastener, etc.] The cut state of the hook-shaped engaging elements of the obtained hook surface fastener was improved compared to that of Comparative Example 1, but some of the hook-shaped engaging elements were cut at a position close to the base, some were cut at a position close to the top, some were left loop-like with the base of one leg not cut, some had both legs cut and were not in a hook shape, and some were cut only partway down one leg. The waviness of this surface fastener was improved compared to Comparative Example 1, but some large waviness was observed, as well as some fine waviness.
[0181] The pull-out force and engagement force of the hook-shaped engaging elements of this hook surface fastener, as well as the state of pull-out of the hook-shaped engaging elements from the surface of the hook surface fastener after 1,000 repeated engagement and peeling cycles, were similar to those of Comparative Example 1. The (Tb) / (Ts) ratio of this hook surface fastener was 0.95. Furthermore, the state of attachment to clothing using the ears of this hook surface fastener with sewing thread was slightly improved compared to that of Comparative Example 1, but the results were almost similar to those of Comparative Example 1.
[0182] Comparative Example 10 [Manufacturing of Loop Hook and Loop Fastener] In Example 5 above, as in Comparative Example 9 above, a loop hook and loop fastener was manufactured by the same method as in Example 5, except that the surface speed of the roll surface was the same as the running speed of the loop hook and loop fastener fabric, and the back surface of the loop hook and loop fastener fabric was pressed onto the roll surface but not sliding on the roll surface.
[0183] [Performance of the obtained loop hook-and-loop fastener, etc.] The (Tb) / (Ts) ratio of the obtained loop hook-and-loop fastener was 0.96, and the pull-out force of the loop-shaped engaging element was 8.8 N, which were similar in performance to those of Comparative Example 2. Furthermore, the waviness of this hook-and-loop fastener in the vertical direction was hardly improved, and many raised areas were observed, similar to those of Comparative Example 2. Furthermore, the engaging force of this loop hook-and-loop fastener and the ease of sewing using the ears were inferior, similar to those of Comparative Example 9.
[0184] Example 10 The hook surface fastener obtained in Example 1, the loop surface fastener obtained in Example 2, and the hook-and-loop coexisting surface fastener obtained in Example 3 were each dyed under the following dyeing conditions to obtain three types of surface fasteners dyed a deep black color. [Dyeing conditions] Dye: Tuxedo Black H (manufactured by Dystar) 7% owf Auxiliaries: Nikka Sunsalt SN130 (manufactured by Nicca Chemical Co., Ltd.) 2g / L, Textport SN10 (manufactured by Nicca Chemical Co., Ltd.) 2g / L, Sunmol 120 1g / L, Acetic acid 2g / L, MYS 0.10% Liquor ratio: 1:15 Dyeing temperature and time: 135°C x 120 minutes (heat from 40°C to 135°C in 30 minutes, and keep at 135°C for 120 minutes) Reduction cleaning: caustic soda 1g / L, thiourea dioxide 0.5g / L, Escudo NEO-2E 1g / L, 80°C x 15 minutes, Water rinsing: 15 minutes, Drying: 60°C x 30 minutes
[0185] All hook-and-loop fasteners were dyed in deep colors, and the dyed products had excellent abrasion fastness and hot water fastness, and were both sufficiently durable for use under harsh conditions. Furthermore, the flame retardancy and engagement force were no different from those before dyeing, and the (Tb) / (Ts) ratio was also no different from those before dyeing.
[0186] 1: Base fabric (loop fabric) 2: Loop for engaging element 3: Heat treatment furnace 4: Fixed surface or roll surface 5: Warp thread 6: Weft thread 7: Hook-shaped engaging element K: Base fabric thickness direction Tb: Thickness of warp thread in the base fabric thickness direction at the point where it sinks most deeply on the back side Ts: Thickness of warp thread in the base fabric thickness direction at the point where it rises most deeply on the front side
Claims
1. a base fabric woven from warp yarns made of polyphenylene sulfide-based multifilament yarns, weft yarns made of multifilament yarns made of polyphenylene sulfide-based multifilament yarns and heat-fusible filaments, and engaging element yarns made of at least one kind selected from the group consisting of polyphenylene sulfide-based multifilament yarns and monofilament yarns; an engaging element formed from the yarn for the engaging element and present on a surface of the base fabric; A hook-and-loop fastener having The flame-retardant hook-and-loop fastener is characterized in that the warp thickness in the base fabric thickness direction at the point where the warp threads, which are floating and sinking above and below the weft thread sandwiched therebetween, are most deeply sunk on the back side is 0.94 times or less the warp thickness in the base fabric thickness direction at the point where the warp threads are most deeply raised on the front side.
2. 2. The flame-retardant hook-and-loop fastener according to claim 1, wherein the warp thickness in the base fabric thickness direction at the point where the warp threads, which are sandwiched between the weft threads and float above and below the weft threads, are most deeply sunk on the back surface side is in the range of 0.70 to 0.90 times the warp thickness in the base fabric thickness direction at the point where the warp threads are most deeply raised on the front surface side.
3. 3. The flame-retardant hook-and-loop fastener according to claim 1 or 2, wherein the weft yarn is an aligned yarn of a polyphenylene sulfide multifilament yarn having a total thickness of 120 to 300 decitex, in which 5 to 90 filaments having a thickness of 3 to 30 decitex are bundled together, and a heat-fusible multifilament yarn having a total thickness of 80 to 150 decitex, in which 15 to 40 polyester sheath-core filaments having a thickness of 3 to 8 decitex are bundled together, the sheath component being a low-melting point heat-fusible component.
4. A flame-retardant hook-and-loop fastener as described in claim 1 or 2, wherein on the surface of the hook-and-loop fastener, engaging element regions in which engaging elements are present and ear regions in which no engaging elements are present are each continuous in the warp direction, and in the weft direction, the engaging element regions and the ear regions alternate, and further, there are multiple engaging element regions.
5. 3. A flame-retardant surface fastener according to claim 1, wherein the engaging elements are hook-shaped engaging elements, and the pulling force of the hook-shaped engaging elements from the base fabric is 5N or more.
6. 3. The flame-retardant hook-and-loop fastener according to claim 1, wherein no backcoat resin layer is present on the back surface of the base fabric.
7. 3. The flame-retardant hook-and-loop fastener according to claim 1, which is colored with a pigment or a disperse dye.
8. a base fabric woven from warp yarns made of polyphenylene sulfide-based multifilament yarns, weft yarns made of polyphenylene sulfide-based multifilament yarns and multifilament yarns made of heat-fusible and heat-shrinkable filaments, and engaging element yarns made of at least one kind selected from the group consisting of polyphenylene sulfide-based multifilament yarns and monofilament yarns; A method for producing a hook-and-loop fastener having at least one type selected from the group consisting of a large number of hook-shaped engaging elements and a large number of loop-shaped engaging elements formed from said yarn for engaging elements, which is present on the surface of a base fabric, A method for producing a flame-retardant hook-and-loop fastener, comprising carrying out the following steps A, B, C and D in this order: [Step A] When weaving a base fabric from warp and weft yarns, a step of weaving an engaging element yarn parallel to the warp yarn and at the same time, regularly straddling the engaging element yarn over the warp yarn, and causing the engaging element yarn to rise in a loop shape from the surface of the base fabric at the straddling points, thereby weaving a loop fabric; [Step B] A step of guiding the loop fabric to a heating zone, heating the loop fabric to a temperature equal to or higher than the temperature at which the heat-fusible component of the multifilament yarn made of the heat-fusible and heat-shrinkable filaments melts, and heat-shrinking the multifilament yarn made of the heat-fusible and heat-shrinkable filaments, thereby fixing the engaging element yarn to the base fabric by the melt from the multifilament yarn made of the heat-fusible and heat-shrinkable filaments; [Step C] A step of removing the loop fabric from the heating zone of step B, and sliding the back surface of the base fabric on a fixed surface or a roll surface while pressing the back surface of the base fabric on the fixed surface or a roll surface while the heat-fusible component of the multifilament yarn composed of the heat-fusible and heat-shrinkable filaments is molten; [Step D] A step of removing the loop fabric from step C, cooling the loop fabric, and then cutting one leg of the loop to form the loop into a hook-shaped engaging element in the case where the yarn for the engaging element is a monofilament yarn;
9. A method for producing a flame-retardant hook-and-loop fastener as described in claim 8, wherein step C is performed by pressing the back side of the loop fabric against the fixed surface while sliding the loop fabric over the same surface, and changing the running direction of the loop fabric over the fixed surface.
10. 10. The method for producing a flame-retardant hook-and-loop fastener according to claim 8 or 9, wherein step C is carried out subsequent to step B, without first cooling the loop fabric removed from step B, by utilizing the residual heat of step B.
11. The method for producing a flame-retardant hook-and-loop fastener according to claim 8 or 9, wherein the dry heat shrinkage rate at 200°C of the multifilament yarn made of heat-fusible and heat-shrinkable filaments is in the range of 10 to 24%.
12. The method for producing a flame-retardant hook-and-loop fastener according to claim 8 or 9, wherein the tension applied to the loop fabric in step C is 50 to 600 g / cm.
13. 10. The method for producing a flame-retardant hook-and-loop fastener according to claim 8 or 9, wherein steps A to D are carried out continuously without winding in between.
14. A method for producing a flame-retardant hook-and-loop fastener as described in claim 8 or 9, in which, in the above-mentioned step A, a loop fabric is woven in which on the surface of the loop fabric, engaging element regions in which engaging element loops are present and ear regions in which no engaging element loops are present are each present continuously in the warp direction, and in which the engaging element regions and ear regions alternate in the weft direction, and further in which a plurality of engaging element regions are present, and after the above-mentioned step D, the centers of the ear regions are slit in the warp direction to simultaneously produce a plurality of hook-and-loop fasteners which are continuous in the warp direction and have ears at both ends.