Method for producing proton-containing oxide, dense body of proton-containing basic composite oxide, solid electrolyte, fuel cell, hydrogen production cell, hydrogen sensor, or ammonia synthesis cell, and methods for producing same
Patent Information
- Application Number
- JP2024511201
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2024-09-24
- Publication Date
- 2024-12-09
- Estimated Expiration
- 2042-11-21
AI Technical Summary
Current methods for producing proton-containing oxides are limited by high-temperature sintering processes, restricting freedom in shape and composition, and are not applicable to dense samples or those easily reduced, with existing ion exchange methods being complex and time-consuming.
A method involving reacting a basic oxide with a carboxylic acid melt having a pKa of 4 or more to introduce protons, allowing for the production of proton-containing oxides at medium temperatures (150-350°C) suitable for various sample forms, including powders and dense bodies, using elements like B, Mg, Al, Li, and Si, and maintaining the crystal structure.
This method enables the efficient production of proton-containing oxides with high freedom in shape and composition, achieving deep proton introduction and stable proton conductivity in the intermediate temperature range of 300-600°C, suitable for applications in solid electrolytes, fuel cells, and sensors.
Abstract
Description
Method for producing proton-containing oxide, dense body of proton-containing basic composite oxide, solid electrolyte, fuel cell, hydrogen production cell, hydrogen sensor or ammonia synthesis cell, and methods for producing these
[0001] The present invention relates to a method for producing a proton-containing oxide, and a method for producing a fuel cell, a hydrogen production cell, a hydrogen sensor, or an ammonia synthesis cell using the proton-containing oxide obtained by the production method. The present invention also relates to a dense body of a proton-containing basic composite oxide, and a solid electrolyte, a fuel cell, a hydrogen production cell, a hydrogen sensor, or an ammonia synthesis cell containing the same.
[0002] Oxides that are thermally and chemically stable in the medium temperature range of about 300 to 600°C and exhibit high proton conductivity are required in various electrochemical devices such as fuel cells, hydrogen production cells, hydrogen sensors, ammonia synthesis cells, etc. However, most of the known proton-conducting oxides are synthesized via a sintering process at high temperatures (about 1000°C), and are therefore limited to specific material systems such as perovskite-type or related crystal systems, or phosphate-based glasses as described in Patent Document 1, for example, which limits the degree of freedom in terms of shape, including crystal structure, and composition.
[0003] Proton-conducting oxides that decompose at high temperatures but are stable up to the medium temperature range of 300 to 600°C are thought to be available in a wide variety of material and crystalline systems, and research and development into their manufacturing methods is underway. For example, Patent Document 2 and Non-Patent Documents 1 and 2 describe that a dense body of proton-conducting oxide that is stable in the medium temperature range can be obtained by electrochemically replacing alkali ions in a specific alkali-containing sample with protons through ion exchange using hydrogen gas and a direct current voltage. However, Patent Document 2 describes the use of a phosphate glass containing an alkali oxide and an oxide of a polyvalent electropositive element that has multiple oxidation states as the sample, and Non-Patent Document 1 describes the use of NaNbWO 6 , Na 3 Zr 2 Si 3 P.O. 12 , NaMgPO 4 , NaLa(PO 4 ) 3, Li 3 Sc 2 (P.O. 4 ) 3 , Li 5 La 3 Nb 2 O 12 In Non-Patent Document 2, the crystals of Na 3 Zr 2 Si 3 P.O. 12 As described in Non-Patent Document 1, NaNbWO 6 When the sample is used, not only is the sodium ion replaced with a proton, but W 6+ +e - →W 5+ The reactions proceed simultaneously, and ion exchange only occurs in the immediate vicinity of the anode, resulting in the easily reduced NaNbWO 6 Furthermore, the electrochemical ion exchange method requires the application of a proton-injecting electrode and an alkali ion-absorbing electrode to an alkaline sample, and therefore cannot be applied to porous or powdered samples.
[0004] Furthermore, Patent Document 3 and Non-Patent Documents 3 and 4 describe a method of substitution with protons utilizing a chemical potential difference. For example, Patent Document 3 describes a method of exchanging lithium ions for protons in a powder of a substituted garnet-type lithium ion conductive oxide that is excellent in lithium ion conductivity and does not contain aluminum, in a solution of a substance having a hydroxyl group or a carboxyl group at 80° C. or higher to obtain a proton-conductive composite oxide, Li 7-x-y H x La 3 Zr 2-y M y O 12 (M is Ta and / or Nb, 3.2<x≦7−y, 0.25<y<2), and it is described that a powder of a composite oxide having a single phase of a garnet-type structure belonging to a cubic system can be obtained. 13.9 Sr 0.1 Zn(GeO 4 ) 4It is described that the powder was immersed in an aqueous acetic acid solution to exchange lithium ions for protons, and a pressure of 2000 MPa was applied to the resulting proton-substituted powder, and a DC voltage was applied in hydrogen to obtain a dense body. 7 La 3 Nb 2 O 12 It is described that a 3 mm thick, fully ion-exchanged dense body was obtained by immersing the dense body in water at room temperature for 14 days. However, the method described in Patent Document 3 is only capable of ion exchange for powder samples and cannot be applied to dense body samples. Furthermore, the method described in Non-Patent Document 3 cannot be applied to oxide samples that are easily reduced, and the process for producing a proton-introduced dense body is impractical. Furthermore, the process is complicated, as it requires applying a proton-introducing electrode and a Li-absorbing electrode to the sample obtained by applying pressure. Furthermore, the method described in Non-Patent Document 4 is also considered impractical because it is only applicable to limited material systems and requires a long time.
[0005] Japanese Patent No. 3905899 Japanese Patent No. 6041606 International Publication No. 2017 / 033865
[0006] Development of solid electrolytes for intermediate-temperature fuel cells: Development of new materials using high-temperature alkali-proton replacement method, Grant-in-Aid for Scientific Research, Research Report, Japan, May 25, 2017, Project No. 15K14126; S. Tsukuda et al., Inorg. Chem. 2017, Vol. 56, No. 22, pp. 13949-13954; T. Wei et al., Chem. Mater. 2017, Vol. 29, No. 4, pp. 1490-1495; L. Truong et al., J. Mater. Chem. A, 2013, Vol. 1, No. 43, pp. 13469-13475
[0007] As described above, research has been conducted into the synthesis of proton-conducting oxides that are stable up to the medium temperature range of 300 to 600°C. However, Patent Documents 1 to 3 and Non-Patent Documents 1 to 4 merely describe methods for producing oxides into which protons have been introduced (hereinafter referred to as "proton-containing oxides"), in which the shape (powder, porous, dense, etc.) and / or composition (crystal structure, etc.) of the sample for introducing protons are limited. There is a demand for the development of an efficient production method that has fewer restrictions on the shape and composition of the applicable sample and enables proton-containing oxides to be obtained more easily.
[0008] Therefore, an object of the present invention is to provide a production method that can be applied to raw materials in any form, such as powder, porous body, or dense body, and that can easily produce a proton-containing oxide. Another object of the present invention is to provide a novel dense body of a proton-containing basic composite oxide that can be obtained by the production method of the present invention. Another object of the present invention is to provide a solid electrolyte, a fuel cell, a hydrogen production cell, a hydrogen sensor, or an ammonia synthesis cell that includes a proton-containing oxide or a dense body of the proton-containing basic composite oxide obtained by the production method of the present invention, and to apply the production methods thereof.
[0009] The above-mentioned problems of the present invention have been solved by the following means. [1] A method for producing a proton-containing oxide, comprising reacting a basic oxide with a carboxylic acid melt having a pKa of 4 or more to introduce protons into the basic oxide to obtain a proton-containing oxide. [2] The method for producing a proton-containing oxide according to [1], wherein the basic oxide is a basic composite oxide containing at least one element selected from the group consisting of B, Mg, Al, Li, Ca, S, La, Sr, P, Ba, Na, and K, and at least one element selected from the group consisting of Si, Ti, Zr, Hf, Lu, Y, and Sc. [3] The method for producing a proton-containing oxide according to [1] or [2], wherein the basic oxide is a garnet-type or Caswell silverite-related type. [4] The method for producing a proton-introduced oxide according to any one of [1] to [3], wherein the carboxylic acid melt is a fatty acid melt. [5] A method for producing a proton-containing oxide according to any one of [1] to [4], wherein the reaction temperature of the reaction is 150 to 350° C. [6] A method for producing a proton-containing oxide according to any one of [1] to [5], wherein the reaction time of the reaction is 1 to 20 hours. [7] A method for producing a proton-containing oxide according to any one of [1] to [6], comprising washing after the reaction. [8] A method for producing a proton-containing oxide according to any one of [1] to [7], wherein the washing is performed using oil or fat. [9] A method for producing a fuel cell, a hydrogen production cell, a hydrogen sensor, or an ammonia synthesis cell, comprising incorporating, as a solid electrolyte, a proton-containing oxide obtained by the method for producing a proton-containing oxide according to any one of [1] to [8].
[10] A dense body of a proton-containing basic composite oxide containing at least one element selected from the group consisting of B, Mg, Al, Li, Ca, S, La, Sr, P, Ba, Na, and K, and at least one element selected from the group consisting of Si, Ti, Zr, Hf, Lu, Y, and Sc, and containing oxide ions.
[11] A solid electrolyte containing the dense body of the proton-containing basic composite oxide according to
[10] .
[12] A fuel cell, a hydrogen production cell, a hydrogen sensor, or an ammonia synthesis cell containing the solid electrolyte according to
[11] .
[0010] According to the production method of the present invention, a proton-containing oxide can be easily obtained by applying the method to raw materials in any form, such as powder, porous body, or dense body. Furthermore, the dense body of the proton-containing basic composite oxide of the present invention is a novel proton-containing basic composite oxide that can be obtained by the production method of the present invention, and has a high degree of design freedom in terms of shape, composition, and electronic conductivity, and can be used as a solid electrolyte for fuel cells, hydrogen production cells, hydrogen sensors, or ammonia synthesis cells.
[0011] The graph shows the free energy change ΔG° when a hydroxide is produced from a simple oxide (Oxide → Hydroxide) plotted against temperature. Oxide 1 is a graph plotting the amount of Na before and after the ion exchange reaction between a basic oxide and a carboxylic acid melt in accordance with an embodiment of the present invention. 2 ZrO 3 The EDS (energy dispersive X-ray spectroscopy) spectrum of Na before proton introduction is shown. 2 ZrO 3 , the upper spectrum is Na 2 ZrO 3 The spectra before and after the proton introduction are shown. 2 ZrO 3 The lower spectrum shows the X-ray diffraction spectrum of Na before proton introduction. 2 ZrO 3 , the upper spectrum is Na 2 ZrO 3 The spectra after proton introduction into Na are shown. 2 ZrO 3 The change in the crystal structure of Na before proton introduction is shown in Fig. 6(a). 2 ZrO 3 , Figure 6(b) is Na 2 ZrO 3LLZ。Al-added LLZ pellets are sintered into LLZ pellets containing Ta. The graph shows the crystal structure after proton introduction into Al-added LLZ. The graph shows the X-ray diffraction spectra of Al-added LLZ before and after the ion exchange reaction. The lower spectrum shows Al-added LLZ before proton introduction, and the upper spectrum shows the spectrum after proton introduction into Al-added LLZ. The graph shows the Raman spectroscopy spectra of Al-added LLZ before and after the ion exchange reaction. The lower spectrum shows Al-added LLZ before proton introduction, and the upper spectrum shows the spectrum after proton introduction into Al-added LLZ. The graph shows the results of depth profile analysis by Raman spectroscopy after the ion exchange reaction of Al-added LLZ and Ta-added LLZ pellet-shaped sintered bodies. ▼ indicates the plot of Ta-added LLZ, and ▲ indicates the plot of Al-added LLZ. The graph shows a fracture surface image of the surface near the surface of Al-added LLZ pellet-shaped sintered body after ion exchange, taken with a scanning electron microscope (SEM). The graph shows the ion exchange reaction characteristics of acidic compounds. The horizontal axis represents the ion exchange reaction temperature, and the vertical axis represents the pKa of the acidic compound, and the relationship between these is plotted. For tests in which protons were introduced to a depth of 10 μm or more, the maximum depth at which proton introduction was confirmed is also shown. This figure shows the results of depth profile analysis by Raman spectroscopy of Al-added LLZ pellet-shaped sintered bodies after the ion exchange reaction. The plots indicate the cases where behenic acid was used at a reaction temperature of 190°C, the plots indicate the cases where adipic acid was used at a reaction temperature of 180°C, and the plots indicate the cases where behenic acid was used at a reaction temperature of 250°C. The X-ray diffraction spectra of Al-added LLZ before and after the ion exchange reaction are shown. The lower spectrum shows the Al-added LLZ before proton introduction, and the upper spectrum shows the spectrum after proton introduction into the Al-added LLZ. Scanning electron microscope (SEM) fracture surface images of the thickness portion near the surface of the Al-added LLZ before and after the ion exchange reaction are shown. The left side shows the Al-added LLZ before proton introduction, and the right side shows the fracture surface image of the thickness portion near the surface of the Al-added LLZ after proton introduction. 1 shows the micro-Raman spectroscopy spectra of Al-doped LLZ before and after the ion exchange reaction. The bottom spectrum shows the Al-doped LLZ before proton introduction, and the other spectra show the spectra after proton introduction into the Al-doped LLZ.The spectra after proton introduction into Al-doped LLZ are shown, from top to bottom, at relative positions from the surface in the thickness direction of the thin film of the sample: 0 μm (surface), 2.3 μm, 25.3 μm, 48.3 μm, 71.3 μm, 85.1 μm, and 87.4 μm (other surface). The results of depth profile analysis by microscopic Raman spectroscopy of Al-doped LLZ after an ion exchange reaction are shown. Error bars indicate standard deviation, and ● indicates the median. The plot shows the electrical conductivity measurement results of Al-doped LLZ before and after an ion exchange reaction. The horizontal axis represents temperature, and the vertical axis represents the common logarithm of electrical conductivity, and the relationship between these is plotted. △ indicates the Al-doped LLZ before proton introduction, and ▲ indicates the plot after proton introduction into Al-doped LLZ.
[0012] In the present invention, a numerical range expressed using "to" means a range that includes the numerical values written before and after "to" as the lower and upper limits.
[0013] [Method for producing a proton-containing oxide] In the method for producing a proton-containing oxide of the present invention (hereinafter also referred to as "the production method of the present invention"), a basic oxide is reacted with a carboxylic acid melt having a pKa of 4 or higher through an ion exchange reaction, whereby cations of the basic oxide are exchanged with protons of the carboxylic acid having a pKa of 4 or higher, and protons are introduced into the basic oxide, thereby producing a proton-containing oxide. The basic oxide and the carboxylic acid melt having a pKa of 4 or higher, the ion exchange reaction, and the washing treatment used in the production method of the present invention will be described below.
[0014] <Basic Oxide> In the production method of the present invention, the term "basic oxide" refers to an oxide that reacts with a carboxylic acid melt having a pKa of 4 or more, as described below, to form a carboxylate. Therefore, the basic oxide is an oxide of at least one of alkali metals, alkaline earth metals, and transition metals in a low oxidation state (+1 or +2). The basic oxide may contain elements other than oxygen, alkali metals, alkaline earth metals, and transition metals in a low acid valence (+1 or +2). Among these, the basic oxide is preferably an oxide of at least one of alkali metals and alkaline earth metals. The basic oxide may be a simple oxide, which is an oxide of a single metal element, or a composite oxide, which is an oxide of two or more metal elements. Among these, a composite oxide (basic composite oxide) is preferable. Of the cations and anions that constitute the basic oxide, the anion may be an anion containing an oxygen atom. Examples of an anion containing an oxygen atom include oxide ions composed only of oxygen atoms, such as [SiO 4 ] 4- , [PO 4 ] 3- or [GeO 4 ] 3- In the present invention, the oxide ion is a polyanion formed of a polyhedron composed of multiple ions, such as O 2-The term "oxide ion" is not limited to the above, but also includes those whose valence is greater than -2 due to the formation of a covalent bond. In the present invention, oxide ions do not refer to oxide ions constituting polyanions. In the present invention, it is preferable to include oxide ions as anions. In the manufacturing method of the present invention, it is preferable that the basic oxide be hydrophilic, from the viewpoint of smoother ion exchange reaction. In the manufacturing method of the present invention, the basic oxide may have a crystalline structure or may be amorphous, but preferably has a crystalline structure. In the present invention, "having a crystalline structure" means that the presence of regions with translational symmetry can be confirmed by X-ray diffraction. In the manufacturing method of the present invention, the shape of the basic oxide is not particularly limited, and basic oxides in the form of powder, porous body, dense body, or laminate of porous body and dense body can be used to obtain the desired proton-containing oxide. Note that a porous body refers to a bulk body having numerous pores (voids), and a dense body refers to a bulk body that is not porous. A dense body typically has the physical property of being impermeable to liquids and gases. In the present invention, a dense body is defined as one having a relative density of 70% or more. The relative density refers to the percentage of the actual density relative to the theoretical density calculated from the crystal structure, lattice constant, and composition. The actual density is a value measured by dividing the mass measured with a weight-equipped electronic balance by the average volume measured with a standard digital caliper (calculated from the average values of diameter and height measured three times). The relative density of the dense body in the present invention is preferably 75% or more, more preferably 80% or more, and even more preferably 85% or more. There is no particular upper limit, and in practice it is 100% or less.
[0015] In the present invention, in order to maintain the framework of the crystal structure after proton introduction into the basic oxide, a basic composite oxide containing at least one highly basic element and at least one less basic element is preferred. Highly basic element species can be selected based on the free energy change ΔG° Oxide → Hydroxide when a hydroxide is produced from a simple oxide. As shown in Figure 1, these elements have a ΔG° Oxide → Hydroxide of -30 kJ / mol or less at room temperature (25°C), and these elements include B, Mg, Al, Li, Ca, S, La, Sr, P, Ba, Na, and K. Low basic element species refer to elements with a high ΔG° Oxide → Hydroxide, but these ΔG° Oxide → Hydroxide relationships cannot be shown due to the lack of known thermodynamic data. Therefore, the free energy change ΔG° of the production of a simple oxide is selected based on the free energy change ΔG°. Oxide As shown in FIG. 2, the oxide phase can be selected based on its chemical stability. Oxide Among elements having a K of −850 kJ / mol or less at room temperature (25° C.), Si, Ti, Zr, Hf, Lu, Y, and Sc, which do not fall under the category of the above-mentioned highly basic elements, fall into this category. Therefore, the basic oxide is preferably a basic composite oxide containing at least one element from B, Mg, Al, Li, Ca, S, La, Sr, P, Ba, Na, and K, and at least one element from Si, Ti, Zr, Hf, Lu, Y, and Sc.
[0016] Among the elements other than oxygen constituting the basic composite oxide, the proportions of B, Mg, Al, Li, Ca, S, La, Sr, P, Ba, Na, and K are preferably 20 to 95 at%, more preferably 30 to 90 at%, and even more preferably 30 to 85 at%, and the proportions of Si, Ti, Zr, Hf, Lu, Y, and Sc are preferably 5 to 80 at%, more preferably 10 to 70 at%, and even more preferably 15 to 70 at%. Note that the basic composite oxide may contain elements other than B, Mg, Al, Li, Ca, S, La, Sr, P, Ba, Na, and K, as well as Si, Ti, Zr, Hf, Lu, Y, and Sc (hereinafter referred to as "other elements"), such as Ta and Ga. The proportion of the other elements in the basic composite oxide other than oxygen is preferably 0 to 33 at %, more preferably 0 to 15 at %. In the above, "at %" refers to a proportion based on the number of elements. From the viewpoint of obtaining a proton-containing oxide in which ion exchange (proton introduction) has occurred deeper inside using the production method of the present invention, the basic composite oxide is preferably composed of O, at least one element selected from B, Mg, Al, Li, Ca, S, La, Sr, P, Ba, Na, and K, and at least one element selected from Si, Ti, Zr, Hf, Lu, Y, and Sc. In other words, it is preferable that the basic composite oxide does not contain elements other than O, B, Mg, Al, Li, Ca, S, La, Sr, P, Ba, Na, and K, and Si, Ti, Zr, Hf, Lu, Y, and Sc.
[0017] In the examples described later, garnet-type Li 7 La 3 Zr 2 O 12 (hereinafter also abbreviated as "LLZ") derivatives, or Caswellsilverite related type Na 2 ZrO 3 However, the basic oxides used in the present invention are not limited to these, and various basic oxides can be used. For example, K 2 Ti 8 O 17Bronze crystals such as Ca 2 Al 2 SiO 7 Examples of the basic oxide include melilite-type crystals such as those mentioned above. The basic oxides may be commercially available or may be synthesized by a conventional method. When preparing the basic oxide by synthesis, there are no particular limitations on the raw materials, mixing, calcination, sintering methods, etc., and the basic oxide can be synthesized by a conventional method. For example, common oxides and carbonates can be used as raw materials, and examples of the methods include mixing using a ball mill or the like, and calcination and sintering using an electric furnace or the like.
[0018] <Carboxylic Acid Melt with pKa of 4 or More> In the production method of the present invention, a carboxylic acid melt with pKa of 4 or more (hereinafter simply referred to as "carboxylic acid melt") refers to a melt of a Bronsted acid having an acid dissociation constant (pKa) of 4 or more at room temperature (25°C) and one or more carboxy groups. The melting point of the carboxylic acid used in the carboxylic acid melt is not particularly limited as long as it is supplied as a melt (liquid carboxylic acid) during heating in the ion exchange reaction. It is preferable that the carboxylic acid be an organic carboxylic acid that can melt without thermal decomposition during heating in the ion exchange reaction. Furthermore, the production method of the present invention uses a carboxylic acid melt as a proton source, which differs from conventional methods that use an aqueous carboxylic acid solution as a proton source. In other words, the production method of the present invention has an advantage in that water is substantially absent from the reaction system of the ion exchange reaction, as described below. The carboxylic acid melt may be a melt of one carboxylic acid or a melt of a mixture of two or more carboxylic acids. When a melt of a mixture of two or more carboxylic acids is used, at least one carboxylic acid must be melted, and the remaining carboxylic acids may be melted or dissolved in the melted carboxylic acid. When a melt of a mixture of two or more carboxylic acids is used, the pKa of the carboxylic acid melt refers to the pKa of the carboxylic acid exhibiting the lowest pKa. For carboxylic acids exhibiting two or more pKas, the lowest pKa of the two or more pKas is taken as the pKa of the carboxylic acid melt. The pKa of the carboxylic acid melt used in the production method of the present invention is 4 or more (4.0 or more), preferably greater than 4.2, more preferably 4.3 or more, and even more preferably 4.4 or more. There is no particular upper limit to the pKa of the carboxylic acid melt, but it is usually 5.5 or less, preferably 5.0 or less. In the present invention, pKa refers to the negative common logarithm (−logKa) of the acid dissociation constant (Ka) in water at room temperature (25° C.) The pKa can be calculated by adding a 0.01 mol / L aqueous solution of sodium hydroxide dropwise to an aqueous solution of a measurement sample (carboxylic acid) and reading the amount of the aqueous solution of sodium hydroxide added dropwise up to the half-equivalent point.For acids that are insoluble in water, the pKa is calculated by multiplying the acid dissociation constant determined by the above-mentioned titration using another solvent in which the acid is soluble (e.g., dimethyl sulfoxide) by a conversion constant calculated using the pKa of an acid that dissolves in both the solvent and water.
[0019] The carboxylic acid melt is preferably a fatty acid melt. In the present invention, the term "fatty acid melt" refers to a melt of a carboxylic acid having a water solubility (number of grams dissolved in 100 g of water at 25°C) of less than 10 g / 100 g. Examples of the fatty acid melt include unsaturated fatty acids having 12 to 22 carbon atoms, such as oleic acid; saturated fatty acids having 12 to 22 carbon atoms, such as stearic acid and behenic acid; and compounds in which two carboxy groups are bonded to a hydrocarbon having 4 to 8 carbon atoms (which may be saturated or unsaturated), such as adipic acid (water solubility: 2.4 g / 100 g). The blending ratio of the carboxylic acid melt to the basic oxide is not particularly limited as long as the ion exchange reaction described below proceeds. It is preferable to use a carboxylic acid melt containing 20 or more equivalents of protons (H in the carboxy group) relative to the content of elements replaceable by protons in the basic oxide, and it is more preferable to use a carboxylic acid melt containing 100 or more equivalents of protons (H in the carboxy group). There is no particular upper limit to the amount, as long as the amount is sufficient to allow the reaction to occur when the basic oxide is immersed in the carboxylic acid melt.
[0020] <Ion exchange reaction between basic oxide and carboxylic acid melt> According to the production method of the present invention, a proton-containing oxide is obtained in which at least a part of the cations of at least one of alkali metals, alkaline earth metals, and transition metals in a low oxidation state (+1 or +2) in the basic oxide is exchanged with protons in the carboxylic acid melt. The ion exchange reaction in which a basic oxide is reacted with a carboxylic acid melt is described below. 7 La 3 Zr 2 O 12The following describes an example of an ion exchange reaction using (LLZ) and a melt of a monocarboxylic acid compound R-COOH (R represents a hydrocarbon group; the same meaning is used hereinafter) as the carboxylic acid melt. However, the ion exchange reaction in the production method of the present invention is not limited to reactions using these compounds. 7 La 3 Zr 2 O 12 The ion exchange reaction between (LLZ) and R-COOH is represented by the following chemical reaction formula, where x is a number that satisfies 0<x≦7. 7 La 3 Zr 2 O 12 +xR-COOH→H x Li 7-x La 3 Zr 2 O 12 +xR-COOLi In the above chemical reaction formula, Li 7 La 3 Zr 2 O 12 At least a portion of the lithium ions in R—COOH are exchanged with protons in R—COOH, and H x Li 7-x La 3 Zr 2 O 12 A proton-containing oxide represented by the formula:
[0021] The production method of the present invention utilizes the above-mentioned ion exchange reaction and has the following excellent advantages (1) and (2). (1) Since the reaction uses the carboxylic acid melt itself as a proton source and solvent, there is no need to use a low-boiling-point solvent such as water or alcohol. Therefore, compared to conventional techniques in which ion exchange is performed using a low-boiling-point solvent such as water or alcohol, a high-temperature reaction can be performed at, for example, 100°C or higher, and the ion exchange reaction rate can be increased. Therefore, the form of the basic oxide is not limited to powder, and a proton-containing oxide can be obtained even from a porous body or a dense body. In particular, even when a dense body is used, it becomes possible to introduce (inject) protons deep into the dense body. (2) Furthermore, since there is no need to use water, hydrated proton species (H3 O + and H 9 O 4 + ) is not generated in principle, and it is thought that the rate of the ion exchange reaction is not determined by these hydrated proton species. Furthermore, when the basic oxide is hydrophilic and the carboxylic acid melt is also hydrophilic, the ion exchange reaction is also less likely to be inhibited. In other words, since the by-product organic carboxylic acid metal salt (R-COOLi) is hydrophobic, the target proton-containing oxide (H x Li 7-x La 3 Zr 2 O 12 ) and the by-products can be easily removed from the surface of the target object by stirring or the like.
[0022] In the production method of the present invention, the reaction between the basic oxide and the carboxylic acid melt may be carried out in any manner as long as an ion exchange reaction occurs between the basic oxide and the carboxylic acid melt, resulting in a proton-containing oxide in which protons are introduced into the basic oxide. Specifically, by placing the basic oxide and the carboxylic acid melt in contact with each other, the ion exchange reaction occurs on the surface of the basic oxide (the surface in contact with the carboxylic acid melt), and the protons introduced by ion exchange on the surface of the basic oxide are thermally diffused into the interior of the basic oxide, thereby obtaining a proton-containing oxide in which protons are introduced into the interior of the basic oxide. This is as will be described in detail in the results shown in Figure 11 and elsewhere below. From the perspective of injecting protons into the basic oxide at a high concentration, it is preferable that the organic carboxylic acid metal salt, a by-product generated by ion exchange on the surface of the basic oxide, is removed from the surface of the proton-containing oxide so that the surface of the proton-containing oxide can be maintained in contact with the carboxylic acid melt.
[0023] The reaction temperature in the ion exchange reaction may be any temperature at which the carboxylic acid melt can be maintained in a molten state or higher, and can be adjusted as appropriate depending on the acid strength (pKa) of the carboxylic acid melt and other factors. From the viewpoint of the rate of the ion exchange reaction, the reaction temperature is preferably 150 to 350°C, more preferably 180 to 300°C, even more preferably 190 to 300°C, and particularly preferably 200 to 300°C. The reaction time in the ion exchange reaction can be adjusted as appropriate depending on the acid strength (pKa) of the carboxylic acid melt and other factors. From the viewpoint of the balance between the rate of the ion exchange reaction and productivity, the reaction time is preferably 1 to 12 hours, more preferably 2 to 10 hours, even more preferably 2 to 8 hours, and particularly preferably 6 to 8 hours. The reaction time in the ion exchange reaction can be adjusted as appropriate depending on the acid strength (pKa) of the carboxylic acid melt and other factors. From the viewpoint of the balance between the rate of the ion exchange reaction and productivity as well as the enhancement of the ion exchange rate, the reaction time is preferably 1 to 20 hours, and more preferably 2 to 18 hours.
[0024] An example of an apparatus for performing an ion exchange reaction between a basic oxide and a carboxylic acid melt is described below using FIG. 3 . However, the present invention is not limited to this example, and the size, shape, number, and the like can be adjusted and modified as appropriate. In the ion exchange reaction apparatus 100 shown in FIG. 3 , a basic oxide 1 is placed on a mesh 3a of a holding device 3 having a mesh 3a and immersed in a reaction vessel 7 containing a carboxylic acid melt 5. The reaction vessel 7 is closed with a lid 9 that can fix the holding device 3 and is placed on a mantle heater 11. In the ion exchange reaction apparatus 100 shown in FIG. 3 , the basic oxide 1 and the portions of the holding device 3 that are visible through the lid 9 and that are immersed in the carboxylic acid melt 5 are indicated by dashed lines. The holding device 3 is preferably made of a chemically inert noble metal, and is preferably made of silver from the viewpoint of its relatively low cost. If the basic oxide 1 is porous or dense, it can be placed directly on the mesh 3a. However, if it is in powder form, it can be compacted by applying a pressure of approximately 0.1 to 50 MPa, placed on the mesh 3a, and used in the manufacturing method of the present invention. The compact will be porous or dense depending on the hardness of the particles constituting the powder. Typically, hard particles result in a porous compact, while soft particles result in a dense compact. Because the LLZ particles used in the examples described below have hard particles, the resulting compact will be porous. The reaction vessel 7 and lid 9 may be made of any chemically inert material, such as quartz. The lid 9 is designed to suppress volatilization of the carboxylic acid melt 5. The gas inside the reaction vessel 7 is preferably replaced with an inert gas such as nitrogen to prevent oxidation of the carboxylic acid melt 5. To perform the ion exchange reaction by heating, the reaction vessel 7 is placed on a temperature-controllable mantle heater 11 as shown in FIG. 3 to heat the carboxylic acid melt 5. For precise temperature control, it is preferable to place a thermocouple (not shown in FIG. 3) for measuring the temperature in the vicinity of the basic oxide 1 in the carboxylic acid melt 5 .To improve the efficiency of the ion exchange reaction, the ion exchange reaction apparatus 100 preferably has a stirring function that constantly stirs the carboxylic acid melt 5. For example, it is preferable to install the reaction vessel 7 in a mantle heater with a stirrer to heat and stir the carboxylic acid melt 5 (not shown in FIG. 3). Since the specific gravity of the by-product organic carboxylic acid metal salt is greater than that of the carboxylic acid melt 5, installing the basic oxide 1 above the carboxylic acid melt 5 facilitates separation of the organic carboxylic acid metal salt from the proton-containing oxide in which protons have been introduced into the basic oxide 1.
[0025] <Cleaning> The melt after the ion exchange reaction (proton introduction treatment) contains high-melting-point organic carboxylic acid metal salts, which adhere to the surface of the proton-containing oxide, and therefore require thorough cleaning. Even using acetone, known for its strong degreasing power, can sometimes result in insufficient cleaning. In the manufacturing method of the present invention, cleaning can be achieved by using oil or fat. Specifically, the melt after the ion exchange reaction (proton introduction treatment) is replaced with oil or fat and heated again at approximately 150°C for a certain period of time while stirring. Any oil or fat containing a highly unsaturated, low-viscosity fatty acid (commonly known as a saturated fatty acid), such as linoleic acid or linolenic acid, can be used, for example, salad oil. Linoleic acid, linolenic acid, and other acids are composed of unsaturated hydrophobic carboxylic acids that are compatible with organic carboxylic acid metal salts due to their similar polarity. They enhance fluidity and can be used as inexpensive cleaning agents. Linoleic acid and linolenic acid have low acidity (pKa values of 4.8 and 5.0, respectively, at room temperature (25°C)), and therefore do not dissolve the proton-containing oxide during this cleaning treatment. In addition, in the heating and stirring washing in oil or fat, the heating temperature and stirring time are not particularly limited as long as washing is performed, and can be appropriately adjusted. After this washing treatment, the proton-containing oxide is rinsed with acetone to obtain a clean oxide after the proton introduction treatment (proton-containing oxide).
[0026] <Proton-containing oxide> The "proton-containing oxide" obtained by the production method of the present invention means a proton-containing oxide in which at least a part of the cations of at least one of alkali metals, alkaline earth metals, and transition metals in a low oxidation state (+1 or +2) in the basic oxide are exchanged with protons by the above-mentioned ion exchange reaction. For example, when Li is used as the basic oxide, 7 La 3 Zr 2 O 12 When (LLZ) is used, H x Li 7-x La 3 Zr 2 O 12 (x is a number satisfying 0<x≦7) is a proton-containing oxide represented by the formula (1), 2 ZrO 3 When using H y Na 2-y ZrO 3 (y is a number satisfying the relationship 0<y<1.5) is obtained. Note that the production method of the present invention "can be applied to a raw material in any form of powder, porous body, or dense body" means that even when a basic oxide in a dense body form, in which it is most difficult to introduce protons into the interior, is used as a raw material, a proton-containing oxide in which protons are introduced at least to a depth of 10 μm or more from the surface can be obtained.
[0027] (Dense body of proton-containing basic composite oxide) According to the production method of the present invention, a dense body of a proton-containing basic composite oxide containing at least one element selected from B, Mg, Al, Li, Ca, S, La, Sr, P, Ba, Na, and K, and at least one element selected from Si, Ti, Zr, Hf, Lu, Y, and Sc, and containing oxide ions (hereinafter, also referred to as "dense body of the proton-containing basic composite oxide of the present invention") can be obtained as a novel proton-containing oxide. The term "dense body of proton-containing basic composite oxide" refers to a dense body of proton-containing oxides containing at least one element selected from B, Mg, Al, Li, Ca, S, La, Sr, P, Ba, Na, and K, and at least one element selected from Si, Ti, Zr, Hf, Lu, Y, and Sc, and in which at least one cation of at least one alkali metal and alkaline earth metal in the basic composite oxide containing oxide ions has been substituted with protons. Thus, the dense body of a proton-introducing body of phosphate-based glass, Li 13.9 Sr 0.1 Zn(GeO 4 ) 4 The dense bodies of the proton-introducing bodies of the above do not contain oxide ions and are not included in the dense bodies of the proton-containing basic composite oxides of the present invention. The dense bodies of the proton-containing basic composite oxides of the present invention have low gas permeability because they are dense bodies, and further contain an element with high basicity (at least one element selected from B, Mg, Al, Li, Ca, S, La, Sr, P, Ba, Na, and K) and an element with low basicity (at least one element selected from Si, Ti, Zr, Hf, Lu, Y, and Sc), and are basic composite oxides containing oxide ions, so that their crystalline structure is resistant to change even after proton introduction and they are stable. For this reason, the dense bodies of the proton-containing basic composite oxides of the present invention are not limited to dense bodies of proton-containing bodies of phosphate-based glasses, Li 13.9 Sr 0.1 Zn(GeO 4 ) 4 Compared to the dense bodies of the proton-introduced bodies, it is a rigid body that does not deform even at high temperatures of 200°C or higher.
[0028] [Solid electrolyte, fuel cell, hydrogen production cell, hydrogen sensor, or ammonia synthesis cell] The proton-containing oxide obtained by the production method of the present invention is expected to exhibit stable proton conductivity in the medium temperature range of 300 to 600° C. Therefore, the proton-containing oxide obtained by the production method of the present invention is expected to be used as a solid electrolyte material, and further, the solid electrolyte obtained from the proton-containing oxide obtained by the production method of the present invention is expected to be used in fuel cells, hydrogen production cells, hydrogen sensors, or ammonia synthesis cells.
[0029] The present invention will be described in more detail below based on examples, but the present invention is not limited to these embodiments except as defined in the present invention.
[0030] [Example 1] (Synthesis of basic oxide) A basic oxide was synthesized by a general firing method as follows. (1) Na 2 ZrO 3 First, as the raw material oxide, ZrO 2 Because of its hygroscopicity, Na was dried at 300°C for 5 hours before being ball milled. 2 CO 3 The mixture was milled with hexane in a planetary ball mill at 400 rpm for 10 hours. The compounding ratio of each oxide in the raw materials was adjusted to a 10 mol% excess of Na relative to the target composition, taking into account sublimation during calcination. Hydrophobic hexane was used to suppress reactions between the raw materials and water (airborne moisture). The resulting mixed powder was pelletized using a uniaxial press into a shape with a diameter of 10 mm and a thickness of 3 mm, then cold isostatically pressed at 20 MPa. The temperature was increased at a rate of 5°C / min in a magnesia crucible, and calcined at 950°C for 12 hours. To prevent contamination of the aluminum, a magnesia crucible was used instead of a typical alumina crucible during calcination. The pellets were calcined while covered with a buffer powder of the same composition to suppress sublimation and unintended reactions. After the calcination, the pellets were ground on both sides, crushed again using a ball mill, pelletized, and fired in the same manner as the calcination. 2ZrO 3 Dense pellets (dense bodies with a relative density of 82% or more) were prepared. The pellets were again pulverized using a ball mill in the same manner as above to prepare powder samples.
[0031] (2) Li 6.16 Al 0.28 La 3 Zr 2 O 12 (Al-doped LLZ) and Li 6 La 3 Zr 1 Ta 1 O 12 Synthesis of dense body and powder of (Ta-added LLZ) The powder of Al-added LLZ and Ta-added LLZ was prepared by the Na 2 ZrO 3 In the preparation of the powder sample, Li was used as the raw material oxide. 2 CO 3 and ZrO 2 And Al 2 O 3 or Ta 2 O 5 Because of its hygroscopicity, La was calcined at 700°C for 5 hours prior to ball milling. 2 O 3 The powders were prepared in the same manner except that the above-mentioned materials were used. The compounding ratio of each oxide of the raw materials was adjusted so that Li was in excess of 10 mol% with respect to the target composition ratio, taking into account sublimation during firing. The dense bodies of Al-added LLZ and Ta-added LLZ were obtained in the process of preparing the powders described above, and were dense pellets of Al-added LLZ and Ta-added LLZ with a diameter of approximately 9 mm and a thickness of 1 mm (dense bodies with a relative density of 82% or more).
[0032] (3) Li 6.16 Al 0.28 La 3 Zr 2 O 12Preparation of a Thin Film (Dense Body) of (Al-Added LLZ) The pellets of Al-added LLZ prepared in (2) above were pulverized using a ball mill in the same manner as in (1) above to prepare a pulverized powder of Al-added LLZ. 3 g of the pulverized powder of Al-added LLZ prepared as above, 0.5 g of polyvinyl butyral (average degree of polymerization: 630), 250 μL of dibutyl phthalate, 100 μL of ethylene glycol, 100 μL of polyoxyethylene (average degree of polymerization: 10) oxyphenyl ether, 2 mL of isopropanol, and 2 mL of toluene were mixed in a mortar to prepare an Al-added LLZ slurry. Using the Al-added LLZ slurry prepared as described above, a green sheet was prepared using a doctor blade with a 500 μm gap. The sheet was heated to 500°C at a heating rate of 2°C / min, held at 500°C for 3 hours, heated to 1200°C at a heating rate of 10°C / min, held at 1000°C for 10 hours, and cooled to room temperature at a heating rate of 10°C / min to prepare a dense Al-added LLZ thin film (a dense body with a relative density of 92±5% or more) with a thickness of approximately 90 μm. Note that the relative density of the thin film prepared by the doctor blade method is reported as a value including a measurement error of ±5% to take into account the measurement error of the volume measured and calculated using standard digital calipers.
[0033] (Immersion of Basic Oxide in Carboxylic Acid Melt (Ion Exchange Reaction)) The Al-doped LLZ pellets and Ta-doped LLZ pellets were immersed in the carboxylic acid melt using a quartz container in an ion exchange apparatus 100, the schematic diagram of which is shown in Figure 3. This container (reaction vessel 7) was installed on a mantle heater 11 equipped with a stirrer to control the temperature and remove the by-product lithium carboxylate from the surface of the basic oxide sample. For a more uniform reaction, the LLZ pellet (basic oxide 1) was placed on a silver holding device 3 with a silver mesh 3a and suspended above the inside of the reaction vessel 7. A thermocouple was also installed near the LLZ pellet (basic oxide 1) in the carboxylic acid melt 5 for accurate temperature control. To prevent deterioration due to oxidation of the carboxylic acid melt 5 and to allow observation of the sample during the reaction, the entire ion exchange apparatus 100 system was placed in a transparent chamber filled with nitrogen. A carboxylic acid containing 100 times or more equivalents of protons (H in the carboxy group) relative to the Li content of the LLZ pellets (basic oxide 1) was charged into a reaction vessel 7. A carboxylic acid melt 5 was prepared using a mantle heater, and the position of the holding device 3 was adjusted so that the LLZ pellets (basic oxide 1) were immersed in the carboxylic acid melt 5, and an ion exchange reaction was carried out. During the reaction, a quartz lid 9 having a through-hole for the holding device 3 was placed over the carboxylic acid melt 5 to prevent evaporation. The powders of Al-added LLZ, Ta-added LLZ, and Na 2 ZrO 3 The immersion in the carboxylic acid melt of 1 was carried out in the same manner as above, except that the powder was lightly uniaxially pressed at approximately 100 kPa to form a green compact having a diameter of about 10 mm and a thickness of about 1 mm, which was then placed on a mesh 3a. The type of carboxylic acid melt used in the ion exchange reaction, the reaction temperature, and the reaction time are as described below in each evaluation.
[0034] (Washing) The LLZ pellets after the ion exchange reaction were washed with cooking oil heated to about 150°C to remove any lithium carboxylate salts potentially remaining on the surface. Specifically, the carboxylic acid melt (containing lithium carboxylate salts) after the reaction in the reaction vessel 7 was replaced with cooking oil heated to about 150°C, and the mixture was heated and stirred at 150°C for about 20 minutes. The LLZ pellets after the ion exchange reaction were then removed from the cooking oil. The LLZ pellets were then ultrasonically cleaned with acetone to obtain clean samples. The compacted powder after the ion exchange reaction was also washed in the same manner as above to remove any sodium carboxylate salts potentially remaining on the surface. The proton-containing oxides thus obtained were evaluated as follows.
[0035] [Evaluation 1] Caswell Silverite-related Na 2 ZrO 3 Regarding derivatives (reaction conditions) Basic oxide: Na 2 ZrO 3 Powder compact, carboxylic acid melt: oleic acid (pKa 5 or higher) melt, reaction temperature: 300°C, reaction time: 2 hours. Figure 4 shows the Na 2 ZrO 3 4 shows the results of qualitative and quantitative analysis of elements by EDS (energy dispersive X-ray spectroscopy). In FIG. 4, the horizontal axis is the energy value (unit: keV) and the vertical axis is the number of counts. From the ratio of the integrated values of the number of counts in the Kα ray of Na (0.99-1.09 keV) and the Lα ray of Zr (1.99-2.09 keV), the Na content of the raw material before proton introduction was 2 ZrO 3 The elemental composition ratio in the oxide was approximately Na:Zr = 4:1 (see the lower spectrum in Figure 4), whereas the elemental composition ratio in the oxide after proton introduction changed to approximately Na:Zr = 2:1 (see the upper spectrum in Figure 4). As shown in Figure 5, the X-ray diffraction analysis results before and after the ion exchange reaction showed that the Caswell silverite-related Na 2 ZrO 3The (002) diffraction peak of Na SiO 2 shifted from 2θ=16.4° (see the lower spectrum in Figure 5) to 2θ=18.2° (see the upper spectrum in Figure 5), which corresponds to an 11% contraction of the interlayer distance according to Bragg's reflection equation. These results are consistent with the results of the Na SiO 2 before proton introduction shown in Figure 6(a). 2 ZrO 3 In the crystal structure, Na 0.5 ZrO 3 Na present between the block layers 1.5 However, as shown in FIG. 6(b), Na 0.75 +H 0.75 In FIG. 6, the dark circles (●) represent oxygen atoms, and the light circles (◯) represent sodium atoms. That is, Na 2 ZrO 3 It can be seen that protons were sufficiently introduced into the compact up to the center (500 μm from the surface).
[0036] [Evaluation 2] Garnet-type Li 7 La 3 Zr 2 O 12 Regarding the (LLZ) derivative-1 (1) (Reaction conditions) Basic oxide: compacted powder of the Al-added LLZ powder prepared in (2) above, Carboxylic acid melt: oleic acid, Reaction temperature: 150°C, Reaction time: 2 hours. As a result of X-ray diffraction analysis before and after the ion exchange reaction, as shown in Figure 7, a shift in the X-ray diffraction peak was observed, and it was confirmed that the above-mentioned Caswell silverite-related type Na 2 ZrO 3 Similarly, it was confirmed that an oxide was obtained in which the crystal structure of Al-doped LLZ was maintained while changing to a structure in which protons were introduced (ion-exchanged). Furthermore, as a result of Raman spectroscopy, as shown in FIG. 8, the O-H stretching vibration peak, which was hardly observed in the raw Al-doped LLZ before proton introduction (before the ion-exchange reaction), increased to approximately 3520 cm after proton introduction (after the ion-exchange reaction). -1 These results suggest that the Al-doped LLZ crystal structure before proton introduction is clearly observed in the vicinity of Li. + Part of it is H +In other words, it can be seen that protons were sufficiently introduced into the compact of the Al-added LLZ powder up to the center of the compact (500 μm from the surface).
[0037] (2) (Reaction Conditions) Basic oxide: dense body of Al-doped LLZ or Ta-doped LLZ prepared in (2) above (relative density 82% or more, porosity approximately 15%), carboxylic acid melt: adipic acid (pKa 4.4), reaction temperature: 180°C, reaction time: 8 hours. The oxides after the ion exchange reaction of each pellet-shaped sintered body of Al-doped LLZ and Ta-doped LLZ (porosity approximately 15%) were analyzed in the depth direction by Raman spectroscopy. The horizontal axis represents the depth from the pellet surface, and the vertical axis represents the O-H stretching vibration peak intensity. The relationship between these is plotted in Figure 9. In the Raman spectroscopy analysis of the present invention, analysis was performed every 10 μm in the depth direction from the surface (depth 0 μm), and the deepest depth at which the O-H stretching vibration peak was no longer observed was determined as the maximum depth at which protons were introduced. As shown in Figure 9, in the Ta-added LLZ (indicated by ▼ in Figure 9), protons were introduced from the surface (0 μm) to a depth of 20 μm, and in the Al-added LLZ (indicated by ▲ in Figure 9), protons were introduced from the surface (0 μm) to a depth of approximately 250 μm. Furthermore, as shown in Figure 10, a scanning electron microscope was used to observe no cracks or other defects on the fracture surface near the surface of the Al-added LLZ pellet-shaped sintered body after the ion exchange reaction. These results confirm that, after ion exchange at the surface of the Al-added LLZ, protons diffused inward, resulting in an oxide with protons introduced all the way to the inside.
[0038] [Evaluation 3] Garnet-type Li 7 La 3 Zr 2 O 12Regarding the (LLZ) Derivative-2 (Reaction Conditions) Basic Oxide: Dense Al-doped LLZ prepared in (2) above (relative density 82% or more, porosity approximately 15%), Reaction Time: 8 hours. Ion exchange reactions were performed using aqueous acetic acid or various carboxylic acid melts as the proton introduction source, with varying reaction temperatures. Surface and depth analysis of the resulting oxides were performed using Raman spectroscopy to measure the O-H stretching vibration peak intensity. Figure 11 plots the relationship between the pKa (room temperature: 25°C) of the compound used as the proton introduction source and the reaction temperature, along with the maximum depth at which proton introduction was confirmed in each test. In Figure 11, "ion exchange only at the surface (<10 μm)" means that an O-H stretching vibration peak was observed in the surface analysis, but no O-H stretching vibration peak was observed at the surface (depth 0 μm) in the depth analysis. "Dissolved in Acid" means that the basic oxide was dissolved in acid. As shown in Figure 11, when an aqueous solution of acetic acid (pKa 4.7) was used at a reaction temperature of 80°C, ion exchange occurred only to a depth of less than 10 µm from the surface. Furthermore, because it was an aqueous solution, the reaction temperature could not be raised above 100°C, making it difficult to introduce protons further into the interior. Furthermore, when an isoleucine-adipic acid melt (pKa 2.3) was used at a reaction temperature of 180°C, when an ethylene-acrylic acid copolymer melt (15 wt% acrylic acid component, pKa 4.2) was used at a reaction temperature of 250°C or 350°C, or when an adipic acid melt (pKa 4.4) was used at a reaction temperature of 250°C, the basic oxide was dissolved by the acid, and the desired proton-containing oxide was not obtained. In contrast, when adipic acid (pKa 4.4) or behenic acid (pKa 4.7), which are carboxylic acid melts with a pKa of 4 or higher, were used, ion exchange could be achieved to a depth of 60 μm or more by setting the reaction temperature at a level at which the basic oxide would not dissolve in the acid. In particular, as shown in Figures 11 and 12, protons could be introduced to a depth of 250 μm with adipic acid at a reaction temperature of 180°C, and to a depth of 60 μm with behenic acid at a reaction temperature of 190°C, and to a depth of 300 μm or more at a reaction temperature of 250°C. Furthermore, in the reaction using behenic acid at a reaction temperature of 250°C, La was produced as the second phase. 2 Zr2 O 7 It was confirmed that protons exist. Considering these results, when an oleic acid melt (pKa 5.0) was used at a reaction temperature of 200°C, ion exchange only occurred within a depth of less than 10 μm from the surface. However, as is clear from the plot in Figure 11, by increasing the reaction temperature, ion exchange can be achieved to a deeper depth. Thus, it was found that by using a weakly acidic carboxylic acid melt with a pKa of 4 or higher at a high temperature, protons can be introduced from the surface to a deeper interior.
[0039] [Evaluation 4] Garnet-type Li 7 La 3 Zr 2 O 12Regarding the (LLZ) Derivative-3 (Reaction Conditions) Basic oxide: Al-doped LLZ thin film (dense body with a relative density of 92±5% or more) prepared in (3) above; Carboxylic Acid Melt: Behenic Acid (pKa 4.7); Reaction Temperature: 250°C; Reaction Time: 15 hours. Samples of the Al-doped LLZ thin film before and after the ion exchange reaction were subjected to ICP-MS (inductively coupled plasma mass spectrometry), X-ray diffraction, SEM (scanning electron microscope), micro-Raman spectroscopy, and AC impedance spectroscopy. [ICP-MS Analysis] Each sample before and after the ion exchange reaction (proton introduction) was ground in a mortar, and then 1 mL of aqua regia was added to 1 mg of the ground powder. The solution was hydrolyzed at 105°C for 2 hours to form a solution, which was then introduced into an ICP-MS system for analysis. ICP-MS analysis confirmed that the Li concentration in the sample after the ion exchange reaction was 1 / 10 of the Li concentration in the sample before the ion exchange reaction, i.e., the ion exchange rate in the ion exchange reaction was 90%. X-ray diffraction revealed a shift in the X-ray diffraction peak, as shown in FIG. 13 , confirming that the ion exchange reaction resulted in an oxide in which the crystal structure of the sample before the ion exchange reaction was maintained while a proton-introduced (ion-exchanged) structure was obtained. SEM observation, as shown in FIG. 14 , confirmed that both the samples before and after the ion exchange reaction were dense bodies free of cracks, open pores, etc. The difference in sample thickness in the SEM images before and after the ion exchange reaction in FIG. 14 is due to the uneven thickness of the sample itself. Micro-Raman spectroscopy revealed, as shown in FIG. 15 , that the O-H stretching vibration peak, which was barely observed in the sample before proton introduction (before the ion exchange reaction), increased to approximately 3520 cm from the surface to the interior of the sample (at relative positions of 0 μm to 87.4 μm) after proton introduction (after the ion exchange reaction). -1 It was observed at about 2840 to 2940 cm -1 A peak thought to be due to O-H stretching vibration was also observed at approximately 3520 cm. -1 The vertical axis represents the O-H stretching vibration peak intensity, and the relationship between these is plotted in Figure 16. As shown in Figure 16, -1It was confirmed that the intensity of the O-H stretching vibration peak was almost constant on the surface and inside of the sample from one surface (relative position 0 μm) to the other surface (relative position 87.4 μm). These results confirmed that after ion exchange on the surface of the Al-doped LLZ thin film, protons diffused inward, resulting in an oxide with an ion exchange rate of 90% and protons uniformly introduced all the way to the inside.
[0040] [AC Impedance Spectroscopy] Platinum paste was applied to a thin film of Al-added LLZ for current collection, and platinum electrodes were connected. The thin film was placed in a tubular furnace and subjected to AC voltage of 100 mV and AC frequency of 2×10 while circulating synthetic air. 7 Impedance spectra were measured while increasing the temperature from 150°C to 400°C in a frequency range of 100 to 0.1 Hz. The point where the impedance spectrum intersects with the real axis in the Nyquist plot was taken as the real resistance value, and was converted to electrical conductivity using the current collection area and sample thickness. The horizontal axis represents the measurement temperature, and the vertical axis represents the common logarithm of the calculated electrical conductivity. Figure 17 shows a plot of these relationships. Regarding electrical conduction, lithium ion conduction was the main component in the Al-added LLZ before ion exchange, while proton conduction was the main component in the Al-added LLZ after ion exchange. As shown in Figure 17, AC impedance spectroscopy showed that the sample after the ion exchange reaction exhibited a conductivity of approximately 1 × 10 at a temperature range of 325°C. -4 S.cm. -1 It was confirmed that the present invention made it possible to easily obtain a proton-containing oxide exhibiting high proton conductivity.
[0041] While the present invention has been described in connection with embodiments thereof, we do not intend to limit our invention to any of the details of the description unless otherwise specified, and believe that the claims should be construed broadly without departing from the spirit and scope of the invention as set forth in the appended claims.
[0042] REFERENCE SIGNS LIST 1 Basic oxide 3 Holding device 3a Mesh 5 Carboxylic acid melt 7 Reaction vessel 9 Lid 11 Mantle heater 100 Ion exchange reaction device
Claims
1. A method for producing a proton-containing oxide, comprising reacting a basic oxide with a molten carboxylic acid having a pKa of 4 or more to introduce protons into the basic oxide, thereby obtaining a proton-containing oxide.
2. 2. The method for producing a proton-containing oxide according to claim 1, wherein the basic oxide is a basic composite oxide containing at least one element selected from the group consisting of B, Mg, Al, Li, Ca, S, La, Sr, P, Ba, Na, and K, and at least one element selected from the group consisting of Si, Ti, Zr, Hf, Lu, Y, and Sc.
3. 3. The method for producing a proton-containing oxide according to claim 1, wherein the basic oxide is a garnet type or a Caswell silverite-related type.
4. The method for producing a proton-containing oxide according to claim 1 or 2, wherein the carboxylic acid melt is a fatty acid melt.
5. The method for producing a proton-containing oxide according to claim 1 or 2, wherein the reaction temperature of the reaction is 150 to 350°C.
6. 3. The method for producing a proton-containing oxide according to claim 1, wherein the reaction time of the reaction is 1 to 20 hours.
7. The method for producing a proton-containing oxide according to claim 1 or 2, further comprising washing after the reaction.
8. The method for producing a proton-containing oxide according to claim 7 , wherein the washing is carried out using oil or fat.
9. A method for producing a fuel cell, a hydrogen production cell, a hydrogen sensor or an ammonia synthesis cell, comprising incorporating, as a solid electrolyte, the proton-containing oxide obtained by the method for producing a proton-containing oxide according to claim 1 or 2.
10. A dense body of a proton-containing basic composite oxide containing at least one element selected from the group consisting of B, Mg, Al, Li, Ca, S, La, Sr, P, Ba, Na, and K, and at least one element selected from the group consisting of Si, Ti, Zr, Hf, Lu, Y, and Sc, and containing oxide ions.
11. A solid electrolyte comprising a dense body of the proton-containing basic composite oxide according to claim 10.
12. A fuel cell, a hydrogen production cell, a hydrogen sensor or an ammonia synthesis cell comprising the solid electrolyte according to claim 11.