Resin composition for ceramic green sheet

JPWO2023189845A5Pending Publication Date: 2024-12-05
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023521860
Authority / Receiving Office
JP · JP
Patent Type
Applications
Priority Date
2023-03-20
Filing Date
2023-03-20
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Current polyvinyl acetal resins used in ceramic green sheets have insufficient solubility in organic solvents and fail to adequately remove finer undissolved substances, leading to decreased productivity in multilayer ceramic capacitors.

Method used

A resin composition for ceramic green sheets is developed, incorporating a polyvinyl acetal resin with specific structural units and a compound A, such as tartaric acid, malic acid, or citric acid, to enhance solvent solubility and reduce undissolved matter, characterized by specific content percentages of hydroxyl, acetyl, and acetal groups, and a compound A content of 2 ppm or more.

Benefits of technology

The resin composition achieves improved solvent solubility and reduced undissolved matter, enabling the production of highly reliable ceramic capacitors with enhanced mechanical strength and processing properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2023189845000001
    Figure 2023189845000001
  • Figure 2023189845000002
    Figure 2023189845000002
Patent Text Reader

Abstract

The present invention provides a resin composition for a ceramic green sheet, the composition having excellent solvent solubility and enabling fabrication of a ceramic capacitor having excellent reliability by reducing the amount of fine undissolved material when dissolved in an organic solvent. The present invention is a resin composition for a ceramic green sheet, the composition containing a polyvinyl acetal resin and a compound A represented by formula (1), wherein the content of the compound A is at least 2 ppm based on weight. In formula (1), R1 and R3 each independently represent a carboxyl group or a salt thereof, and R2 represents a single bond or a divalent group that may be substituted by at least one substituent selected from the group consisting of hydroxyl groups, carboxyl groups, and salts thereof.
Need to check novelty before this filing date? Find Prior Art

Description

Resin composition for ceramic green sheet

[0001] The present invention relates to a resin composition for a ceramic green sheet.

[0002] In recent years, electronic components mounted in various electronic devices have become increasingly miniaturized and multilayered, resulting in widespread use of multilayer electronic components such as multilayer circuit boards, laminated coils, and multilayer ceramic capacitors. Multilayer ceramic capacitors, among others, are generally manufactured through the following process. First, a plasticizer, dispersant, etc. are added to a solution of a binder resin, such as polyvinyl butyral resin or poly(meth)acrylate resin, dissolved in an organic solvent. Then, ceramic raw material powder is added and uniformly mixed using a mixing device such as a bead mill or ball mill. After degassing, a ceramic slurry composition with a constant viscosity is obtained. This slurry composition is cast onto a support surface, such as a release-treated polyethylene terephthalate film or SUS plate, using a doctor blade or reverse roll coater. The resulting ceramic green sheets are then heated to remove volatiles such as the solvent, and the sheets are peeled off from the support to obtain ceramic green sheets. Next, multiple sheets of the resulting ceramic green sheets, each coated with a conductive paste for internal electrodes by screen printing, are stacked alternately and then heated and pressed together to form a laminate. Thereafter, the laminate is subjected to a process of thermally decomposing and removing binder resin components and the like contained in the laminate, a so-called degreasing process, and then external electrodes are sintered onto the end faces of the ceramic sintered body obtained by firing, to obtain a multilayer ceramic capacitor.

[0003] For example, Patent Document 1 describes a polyvinyl acetal resin suitable as a ceramic binder, which has a predetermined degree of polymerization, vinyl ester unit content, and degree of acetalization, and in which the molar ratio of the portion acetalized with acetaldehyde to the portion acetalized with butylaldehyde is within a predetermined range. Also, Patent Document 2 describes a polyvinyl acetal resin having a predetermined degree of polymerization, vinyl ester unit content, and degree of acetalization, and having specific structural units.

[0004] JP 2011-236304 A International Publication No. 2012 / 023517

[0005] On the other hand, in recent years, with the increasing functionality and miniaturization of electronic devices, multilayer ceramic capacitors are being required to have higher capacitance and be smaller in size. To meet such demands, it is necessary to thoroughly remove finer undissolved matter. However, even the polyvinyl acetal resins described in Patent Documents 1 and 2 are unable to sufficiently remove finer undissolved matter, and the undissolved matter must be removed by filtration or the like, resulting in a problem of reduced productivity. Furthermore, even the polyvinyl acetal resins described in Patent Documents 1 and 2 have the problem of insufficient solubility in organic solvents.

[0006] An object of the present invention is to provide a resin composition for ceramic green sheets that has excellent solvent solubility and, when dissolved in an organic solvent, reduces the amount of fine undissolved matter, thereby enabling the production of highly reliable ceramic capacitors.

[0007] The present disclosure (1) is a resin composition for a ceramic green sheet, comprising a polyvinyl acetal resin and a compound A represented by the following formula (1), wherein the content of the compound A is 2 ppm or more by weight: In formula (1), R 1 and R 3 each independently represents a carboxyl group or a salt thereof, R 2 represents a single bond or a divalent group which may be substituted with at least one substituent selected from the group consisting of a hydroxyl group, a carboxyl group, and salts thereof. 2 is a linear alkylene group having 1 to 6 carbon atoms which may be substituted with at least one substituent selected from the group consisting of a hydroxyl group, a carboxyl group, and salts thereof. 2is a linear alkylene group having 1 to 3 carbon atoms and having at least one selected from the group consisting of a hydroxyl group, a carboxyl group, and salts thereof. The present disclosure (4) is a resin composition for a ceramic green sheet, which is an arbitrary combination with any of the present disclosures (1) to (3), in which X represented by the following formula (2) is 1.6 or more and 4.5 or less: Disclosure (5) is a resin composition for a ceramic green sheet, which is any combination with any of Disclosures (1) to (4), in which Compound A is at least one compound selected from the group consisting of tartaric acid, malic acid, citric acid, and salts thereof. Disclosure (6) is a resin composition for a ceramic green sheet, which is any combination with any of Disclosures (1) to (5), in which the polyvinyl acetal resin has a solution viscosity of 50 mPa·s or more at 20°C when dissolved at 10 wt% in an ethanol / toluene mixed solution (weight ratio 1:1). Disclosure (7) is a resin composition for a ceramic green sheet, which is any combination with any of Disclosures (1) to (6), in which the polyvinyl acetal resin has an acetyl group content of 0.5 wt% or more and 20 wt% or less. Disclosure (8) is a resin composition for a ceramic green sheet, which is any combination with any of Disclosures (1) to (7), in which the polyvinyl acetal resin has an average degree of polymerization of 500 or more. The present invention will be described in detail below.

[0008] As a result of extensive research, the present inventors have found that by adding a predetermined amount of compound A having a specific structure to a polyvinyl acetal resin to form a resin composition, it is possible to produce a ceramic capacitor that has excellent solvent solubility, reduces the amount of fine undissolved matter when dissolved in an organic solvent, and is therefore highly reliable, and have completed the present invention.

[0009] The resin composition for a ceramic green sheet contains a polyvinyl acetal resin. The polyvinyl acetal resin typically has a structural unit having a hydroxyl group represented by the following formula (a-1), a structural unit having an acetyl group represented by the following formula (a-2), and a structural unit having an acetal group represented by the following formula (a-3).

[0010]

[0011] In the above formula (a-3), R 1a represents a hydrogen atom or an alkyl group having 1 to 20 carbon atoms.

[0012] Examples of the alkyl group having 1 to 20 carbon atoms include a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, a heptyl group, an octyl group, a nonyl group, a decyl group, an undecyl group, a dodecyl group, a tridecyl group, a tetradecyl group, a pentadecyl group, a hexadecyl group, a heptadecyl group, an octadecyl group, a nonadecyl group, an eicosyl group, etc. Of these, a methyl group, an ethyl group, and a propyl group are preferred.

[0013] The content of the hydroxyl group-containing structural unit represented by formula (a-1) in the polyvinyl acetal resin (hereinafter referred to as "hydroxyl group content") is preferably 11% by weight or more, more preferably 13% by weight or more, and even more preferably 15% by weight or more, since this can improve the toughness of the resin. Furthermore, since this can further improve solvent solubility, it is preferably 40% by weight or less, more preferably 35% by weight or less, and even more preferably 30% by weight or less. The hydroxyl group content is preferably 11 to 40% by weight, more preferably 13 to 35% by weight, and even more preferably 15 to 30% by weight. The hydroxyl group content can be determined, for example, by measuring the content (mol%) of each structural unit by NMR and calculating the weight ratio.

[0014] The content of the acetyl group-containing structural unit represented by formula (a-2) in the polyvinyl acetal resin (hereinafter referred to as the "acetyl group content") is preferably 0.5% by weight or more, more preferably 0.7% by weight or more, even more preferably 0.8% by weight or more, and even more preferably 1% by weight or more, since this can prevent an increase in viscosity. Furthermore, since this can prevent excessive increase in the flexibility of the polyvinyl acetal resin and improve handleability, it is preferably 30% by weight or less, more preferably 26% by weight or less, even more preferably 22% by weight or less, and even more preferably 20% by weight or less. The acetyl group content is preferably 0.5 to 30% by weight, more preferably 0.7 to 26% by weight, even more preferably 0.8 to 22% by weight, and even more preferably 1 to 20% by weight. The acetyl group content can be determined, for example, by measuring the content (mol%) of each structural unit by NMR and calculating the weight ratio.

[0015] The content of the structural unit having an acetal group represented by formula (a-3) in the polyvinyl acetal resin (hereinafter referred to as the "acetal group amount") is preferably 45% by weight or more, more preferably 47% by weight or more, and even more preferably 49% by weight or more, because this can further improve solubility in solvents. Furthermore, the content is preferably 86% by weight or less, more preferably 85% by weight or less, and even more preferably 83% by weight or less, because this can improve the toughness of the resin. The acetal group amount is preferably 45 to 86% by weight, more preferably 47 to 85% by weight, and even more preferably 49 to 83% by weight. The acetal group amount can be determined, for example, by measuring the content (mol %) of each structural unit by NMR and calculating the weight ratio. Regarding the method for calculating the acetal group amount, since the acetal group of the polyvinyl acetal resin is obtained by acetalizing two hydroxyl groups of polyvinyl alcohol, a method can be adopted in which a structural unit having an acetal group is counted as two structural units having hydroxyl groups.

[0016] The polyvinyl acetal resin may have other structural units in addition to the structural units (a-1), (a-2), and (a-3). Examples of the other structural units include structural units having functional groups such as carboxyl groups, sulfonic acid groups, alkylene oxide groups, and amide groups, and ethylene units.

[0017] Examples of the structural unit having a carboxyl group include a structural unit represented by the following formula (b-1), a structural unit represented by the following formula (b-2), and a structural unit represented by the following formula (b-3).

[0018]

[0019] In the above formula (b-1), R 1b and R 2b each independently represents an alkylene group having 0 to 10 carbon atoms; X 1b and X 2b each independently represents a hydrogen atom, a metal atom, or a methyl group.

[0020] In the above formula (b-1), R 1b and R 2b The lower limit of the number of carbon atoms in the alkylene group represented by the formula (I) is preferably 0, the upper limit is preferably 5, the lower limit is more preferably 1, and the upper limit is more preferably 3. 1b and R 2b may be the same or different, but are preferably different. It is also preferable that at least one of them is a single bond.

[0021] Examples of the alkylene group having 0 to 10 carbon atoms include a single bond, a methylene group, an ethylene group, a trimethylene group, a tetramethylene group, a pentamethylene group, a hexamethylene group, an octamethylene group, a decamethylene group, and other linear alkylene groups, a methylmethylene group, a methylethylene group, a 1-methylpentylene group, a 1,4-dimethylbutylene group, and other branched alkylene groups, and a cyclopropylene group, a cyclobutylene group, a cyclohexylene group, and other cyclic alkylene groups. Of these, a single bond, a methylene group, an ethylene group, an n-propylene group, an n-butylene group, and other linear alkylene groups are preferred, and a single bond, a methylene group, and an ethylene group are more preferred.

[0022] In the above formula (b-1), X 1b and X 2b When at least one of the groups is a metal atom, examples of the metal atom include a sodium atom, a lithium atom, a potassium atom, etc. Among these, a sodium atom is preferred.

[0023] The structural unit represented by the above formula (b-1) is preferably derived from an α-dicarboxy monomer. Examples of the α-dicarboxy monomer include dicarboxylic acids having a radically polymerizable unsaturated double bond, such as methylenemalonic acid, itaconic acid, 2-methyleneglutaric acid, 2-methyleneadipic acid, and 2-methylenesebacic acid, as well as metal salts and methyl esters thereof. Of these, itaconic acid, metal salts, and methyl esters thereof are preferably used. In this specification, the term "α-dicarboxy monomer" refers to a monomer having two carboxyl groups at the α-carbon position.

[0024] In the above formula (b-2), R 3b , R 4b and R 5b each independently represents a hydrogen atom or an alkyl group having 1 to 10 carbon atoms; R 6b represents an alkylene group having 0 to 10 carbon atoms; X 3b represents a hydrogen atom, a metal atom or a methyl group.

[0025] In the above formula (b-2), R 3b , R 4b and R 5b The lower limit of the number of carbon atoms in the alkyl group represented by the formula (I) is preferably 1, the upper limit is preferably 5, and the upper limit is more preferably 3. The number of carbon atoms is preferably 1 to 5, and more preferably 1 to 3.

[0026] R 3b , R 4b , R 5b may be the same or different, but are preferably the same. 3b , R 4b and R 5b is preferably a hydrogen atom.

[0027] Examples of the alkyl group having 1 to 10 carbon atoms include linear alkyl groups such as methyl, ethyl, propyl, n-butyl, n-pentyl, n-heptyl, n-octyl, n-nonyl, and n-decyl, branched alkyl groups such as isopropyl, isobutyl, sec-butyl, tert-butyl, isopentyl, 2,2-dimethylpropyl, 1,1,3,3-tetramethylbutyl, and 2-ethylhexyl, and cycloalkyl groups such as cyclopropyl, cyclopropylmethyl, cyclobutyl, cyclopentyl, and cyclohexyl. Of these, linear alkyl groups such as methyl, ethyl, propyl, and n-butyl are preferred, with methyl and ethyl being more preferred.

[0028] R in the above formula (b-2) 6b As the group, R in the above formula (b-1) 1b and R 2b Among these, a single bond, a methylene group, an ethylene group, a trimethylene group, a tetramethylene group, or other linear alkylene group is preferred, a single bond, a methylene group, or an ethylene group is more preferred, and a single bond is still more preferred.

[0029] In the above formula (b-2), X 3b When is a metal atom, examples of the metal atom include a sodium atom, a lithium atom, a potassium atom, etc. Among these, a sodium atom is preferred.

[0030] The structural unit represented by formula (b-2) is preferably derived from a monocarboxy monomer. Examples of the monocarboxy monomer include monocarboxylic acids having a radically polymerizable unsaturated double bond, such as acrylic acid, crotonic acid, methacrylic acid, and oleic acid, as well as metal salts and methyl esters thereof. Among these, crotonic acid, metal salts, and methyl esters thereof are preferably used.

[0031] In the above formula (b-3), R 7b and R 9b each independently represents a hydrogen atom or an alkyl group having 1 to 10 carbon atoms; R 8b and R 10b represents an alkylene group having 0 to 10 carbon atoms; X4b and X 5b represents a hydrogen atom, a metal atom or a methyl group.

[0032] In the above formula (b-3), R 7b and R 9b The lower limit of the number of carbon atoms in the alkyl group represented by the formula (I) is preferably 1, the upper limit is preferably 5, and the upper limit is more preferably 3. The number of carbon atoms is preferably 1 to 5, and more preferably 1 to 3.

[0033] The above R 7b and R 9b may be the same or different, but it is more preferable that they are the same.

[0034] R in the above formula (b-3) 7b and R 9b As the group, R in the above formula (b-2) 3b , R 4b and R 5b Among them, a hydrogen atom is preferred.

[0035] R in the above formula (b-3) 8b and R 10b As the group, R in the above formula (b-1) 1b and R 2b Among these, a single bond, a methylene group, an ethylene group, a trimethylene group, a tetramethylene group, or other linear alkylene group is preferred, a single bond, a methylene group, or an ethylene group is more preferred, and a single bond is still more preferred.

[0036] In the above formula (b-3), X 4b and X 5b When is a metal atom, examples of the metal atom include a sodium atom, a lithium atom, a potassium atom, etc. Among these, a sodium atom is preferred.

[0037] Examples of the structural unit having a sulfonic acid group include a structural unit represented by the following formula (c).

[0038]

[0039] In formula (c), R 1c represents an alkylene group having 0 to 10 carbon atoms; X 1crepresents a hydrogen atom, a metal atom or a methyl group.

[0040] R in the above formula (c) 1c As the group, R in the above formula (b-1) 1b and R 2b Among these, a single bond, a methylene group, an ethylene group, a trimethylene group, a tetramethylene group, or other linear alkylene group is preferred, a single bond, a methylene group, or an ethylene group is more preferred, and a single bond or a methylene group is even more preferred.

[0041] In the above formula (c), X 1c When is a metal atom, examples of the metal atom include a sodium atom, a lithium atom, a potassium atom, etc. Among these, a sodium atom is preferred.

[0042] Examples of the structural unit having an alkylene oxide group include a structural unit represented by the following formula (d).

[0043]

[0044] In formula (d), R d1 represents a group having an alkylene oxide group having 2 to 6 carbon atoms.

[0045] Examples of the alkylene oxide group having 2 to 6 carbon atoms include an ethylene oxide group, a propylene oxide group, a butylene oxide group, a pentylene oxide group, and a hexylene oxide group. Examples of structural units having an alkylene oxide group represented by formula (d) include those having multiple ethylene oxide groups such as polyethylene glycol, those having a single ethylene oxide group, and those having different alkylene oxide groups.

[0046] The structural unit having an alkylene oxide group is preferably a structural unit having an ethylene oxide group represented by the following formula (e-1), or a structural unit having an ethylene oxide group and a propylene oxide group represented by the following formula (e-2):

[0047]

[0048] In the above formula (e-1), Re1 and R e2 represents a linking group having at least one selected from the group consisting of C and O or a single bond, n 1 represents an integer.

[0049] The above R e1 is a linking group having at least one selected from the group consisting of C and O, or a single bond. e1 is preferably an alkylene group having 1 to 10 carbon atoms, a carbonyl group, or an oxygen atom. e1 Examples of the R include a methylene group, an ethylene group, a carbonyl group, an ether group, an allyl ether group, and an amide group. e2 is a linking group having at least one selected from the group consisting of C and O, or a single bond. e2 is preferably an alkylene group having 1 to 10 carbon atoms, a carbonyl group, or an oxygen atom. e2 Examples of the alkylene group include a methylene group, an ethylene group, a propylene group, a carbonyl group, and an ether group. 1 is not particularly limited, but is preferably 2 to 70, and more preferably 5 to 50.

[0050] In the above formula (e-2), R e3 , R e4 and R e5 represents a linking group having at least one selected from the group consisting of C and O or a single bond, n 2 and n 3 represents an integer.

[0051] The above R e3 , R e4 and R e5 As the group, R in the above formula (e-1) e1 and R e2 The same as those exemplified above can be used. In addition, the integer n, which is the number of repeating alkylene oxides, can be used. 2 , n 3 is not particularly limited, but 2 is preferably 1 to 40, more preferably 20 to 30. 3 is preferably 1 to 40, and more preferably 20 to 30.

[0052] Examples of the structural unit having an amide group include a structural unit represented by the following formula (f).

[0053]

[0054] In the above formula (f), R 1f represents an alkyl group having 1 to 10 carbon atoms.

[0055] R in the above formula (f) 1f As the group, R in the above formula (b-2) 3b , R 4b and R 5b Among them, a hydrogen atom, a methyl group, an ethyl group, a propyl group, an n-butyl group and other linear alkyl groups are preferred, and a hydrogen atom, a methyl group, and an ethyl group are more preferred.

[0056] The content of the structural unit having the functional group in the polyvinyl acetal resin is preferably 0% by weight or more, more preferably 0.1% by weight or more, even more preferably 0.5% by weight or more, and preferably 5% by weight or less, more preferably 3% by weight or less. The content of the structural unit having the functional group is preferably 0 to 5% by weight, more preferably 0.1 to 3% by weight, and even more preferably 0.5 to 3% by weight. The content of the structural unit having the functional group can be determined, for example, by measuring the content (mol%) of each structural unit by NMR and calculating the weight ratio.

[0057] The ethylene unit may be a structural unit represented by the following formula (g).

[0058]

[0059] In the polyvinyl acetal resin, the content of the ethylene unit (hereinafter also referred to as "ethylene content") is preferably 1% by weight or more, more preferably 3% by weight or more, and preferably 20% by weight or less, more preferably 10% by weight or less. The ethylene content is preferably 1 to 20% by weight, more preferably 3 to 10% by weight. The ethylene content can be determined, for example, by measuring the content (mol %) of each structural unit by NMR and calculating the weight ratio.

[0060] In this specification, the ethylene content of a polyvinyl acetal resin means the apparent ethylene content of the entire polyvinyl acetal resin. That is, for example, when a polyvinyl acetal resin contains multiple resins having different ethylene contents, the ethylene content of the polyvinyl acetal resin can be determined by multiplying the ethylene content of each resin by the content ratio of that resin and adding up the resulting values.

[0061] In the polyvinyl acetal resin, the ratio of the ethylene content to the hydroxyl group content (ethylene content / hydroxyl group content) is preferably 0.01 or more and 1.0 or less. The ratio is preferably 0.01 to 1.0.

[0062] The average degree of polymerization of the polyvinyl acetal resin is preferably 200 or more, more preferably 300 or more, as this allows for improved mechanical strength. Furthermore, from the viewpoints of solvent solubility and viscosity, it is preferably 500 or more, more preferably 10,000 or less, and even more preferably 5,500 or less. The average degree of polymerization is preferably 200 to 10,000, more preferably 300 to 5,500, and even more preferably 500 to 5,500. The average degree of polymerization is the same as that of the raw material polyvinyl alcohol resin. The average degree of polymerization of the raw material polyvinyl alcohol resin can be measured in accordance with JIS K 6726.

[0063] The polyvinyl acetal resin preferably has a solution viscosity at 20°C of 10% by weight dissolved in an ethanol / toluene mixed solution (1:1 by weight) of 50 mPa·s or more, more preferably 70 mPa·s or more, and even more preferably 100 mPa·s or more, and preferably 20,000 mPa·s or less, more preferably 18,000 mPa·s or less, and even more preferably 16,000 mPa·s or less. The viscosity is preferably 50 to 20,000 mPa·s, more preferably 70 to 18,000 mPa·s, and even more preferably 100 to 16,000 mPa·s. Setting the viscosity within the above range ensures uniform solvent solubility and improves mechanical strength. The viscosity can be measured, for example, using a Brookfield viscometer at a solution temperature of 20°C.

[0064] The shape of the polyvinyl acetal resin is not particularly limited, but is preferably particulate. Furthermore, when the polyvinyl acetal resin is particulate, the solubility in organic solvents can be further increased, so the porosity is preferably 20% or more, more preferably 25% or more, and even more preferably 30% or more, and is preferably 80% or less, more preferably 70% or less, and even more preferably 60% or less. The porosity is preferably 20 to 80%, more preferably 25 to 70%, and even more preferably 30 to 60%. The porosity refers to the volume of pores with a pore radius of 0.0038 to 7.5 μm relative to the volume of the resin particles. The porosity can be measured, for example, by mercury intrusion porosimetry using a porosimeter (Thermo Pascal 14B, manufactured by Thermo Fisher Scientific). The porosity can be adjusted by adjusting the concentration of the polyvinyl alcohol resin or the stirring conditions in the acetalization step, or by adjusting the temperature in the neutralization step of the obtained resin particles. For example, the porosity of the obtained resin particles increases when the polyvinyl alcohol concentration relative to the amount of pure water during the acetalization reaction is lower.

[0065] When the polyvinyl acetal resin is in a particulate form, the solubility in organic solvents can be further increased. 2 / g or more, and 2 / g or more, and 15m 2 / g or more is more preferable, and 30m 2 / g or less, and 2 / g or less is more preferable, and 20m 2 The specific surface area is more preferably 10 to 30 m / g or less. 2 / g is preferred, and 12 to 25m 2 / g is more preferable, and 15 to 20m 2 In this specification, the specific surface area refers to the surface area per unit weight, and can be measured by mercury intrusion porosimetry using, for example, a porosimeter (Thermo Pascal 14B, manufactured by Thermo Fisher Scientific).

[0066] When the polyvinyl acetal resin is in a particulate form, the solubility in organic solvents can be further enhanced, so the D50 particle size is preferably 30 μm or more, more preferably 50 μm or more, and even more preferably 100 μm or more, and is preferably 800 μm or less, more preferably 600 μm or less, and even more preferably 500 μm or less. The D50 particle size is preferably 30 to 800 μm, more preferably 50 to 600 μm, and even more preferably 100 to 500 μm. The D90 particle size is preferably 30 μm or more, more preferably 50 μm or more, and even more preferably 100 μm or more, and is preferably 1000 μm or less, more preferably 900 μm or less, and even more preferably 800 μm or less. The D90 particle size is preferably 30 to 1000 μm, more preferably 50 to 900 μm, and even more preferably 100 to 800 μm. Furthermore, the D10 particle size is preferably 10 μm or more, more preferably 20 μm or more, and even more preferably 30 μm or more, and is preferably 400 μm or less, more preferably 300 μm or less, and even more preferably 200 μm or less. The D10 particle size is preferably 10 to 400 μm, more preferably 20 to 300 μm, and even more preferably 30 to 200 μm. The "D90 particle size (D90)" refers to the particle size at which the cumulative frequency of the distribution from the small particle side reaches 90% in particle size distribution measurement, while the "D50 particle size (D50)" refers to the particle size at which the cumulative frequency of the distribution reaches 50%, and the "D10 particle size (D10)" refers to the particle size at which the cumulative frequency of the distribution reaches 10%. The D90, D50, and D10 can be measured, for example, using a laser diffraction particle size distribution analyzer (Mastersizer 3000, manufactured by Malvern Panalytical). Methods for controlling the particle size include adjusting the concentration and stirring conditions of the polyvinyl alcohol resin in the acetalization step, and adjusting the temperature and concentration in the neutralization step of the resulting resin particles. Furthermore, for example, the higher the polyvinyl alcohol concentration relative to the amount of pure water during the acetalization reaction, the larger the D50 of the resulting resin particles.

[0067] When the polyvinyl acetal resin is in a particulate form, the particle size distribution ε of the particles is preferably 0.01 or more, more preferably 0.50 or more, and is preferably 4.00 or less, more preferably 3.00 or less. The particle size distribution ε is preferably 0.01 to 4.00, more preferably 0.50 to 3.00. The particle size distribution ε is calculated from [(D90-D10) / D50].

[0068] The content of the polyvinyl acetal resin in the resin composition for a ceramic green sheet is preferably 94% by weight or more, more preferably 95% by weight or more, and even more preferably 96% by weight or more, and is preferably 99.99% by weight or less, more preferably 99.5% by weight or less, and even more preferably 99% by weight or less. The content is preferably 94 to 99.99% by weight, more preferably 95 to 99.5% by weight, and even more preferably 96 to 99% by weight.

[0069] The polyvinyl acetal resin can usually be produced by acetalizing a polyvinyl alcohol resin.

[0070] The polyvinyl alcohol resin can be, for example, a conventionally known polyvinyl alcohol resin, such as a resin produced by saponifying a polyvinyl acetate resin with an alkali, an acid, aqueous ammonia, or the like. The polyvinyl alcohol resin can be fully saponified, but it does not need to be fully saponified as long as it has at least one unit having two consecutive hydroxyl groups at the meso and racemo positions at at least one location on the main chain; it can also be a partially saponified polyvinyl alcohol resin. Furthermore, the polyvinyl alcohol resin can also be a copolymer of vinyl alcohol and a monomer copolymerizable with vinyl alcohol, such as an ethylene-vinyl alcohol copolymer resin or a partially saponified ethylene-vinyl alcohol copolymer resin. Examples of the polyvinyl acetate resin include ethylene-vinyl acetate copolymers.

[0071] The saponification degree of the polyvinyl alcohol resin is preferably 80 mol% or more, more preferably 88 mol% or more, and is preferably 99.4 mol% or less, more preferably 99 mol% or less. The saponification degree is preferably 80 to 99.4 mol%, more preferably 88 to 99 mol%.

[0072] The acetalization can be carried out using known methods, and is preferably carried out in an aqueous solvent, a mixed solvent of water and a water-compatible organic solvent, or an organic solvent. Examples of the water-compatible organic solvent include alcohol-based organic solvents. Examples of the organic solvent include alcohol-based organic solvents, aromatic organic solvents, aliphatic ester-based solvents, ketone-based solvents, lower paraffin-based solvents, ether-based solvents, amide-based solvents, and amine-based solvents. Examples of the alcohol-based organic solvent include methanol, ethanol, n-propanol, isopropanol, n-butanol, and tert-butanol. Examples of the aromatic organic solvent include xylene, toluene, ethylbenzene, and methyl benzoate. Examples of the aliphatic ester-based solvent include methyl acetate, ethyl acetate, butyl acetate, methyl propionate, ethyl propionate, methyl butyrate, ethyl butyrate, methyl acetoacetate, and ethyl acetoacetate. Examples of the ketone solvents include acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, methylcyclohexanone, benzophenone, and acetophenone. Examples of the lower paraffin solvents include hexane, pentane, octane, cyclohexane, and decane. Examples of the ether solvents include diethyl ether, tetrahydrofuran, ethylene glycol dimethyl ether, ethylene glycol diethyl ether, and propylene glycol diethyl ether. Examples of the amide solvents include N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, and acetanilide. Examples of the amine solvents include ammonia, trimethylamine, triethylamine, n-butylamine, di-n-butylamine, tri-n-butylamine, aniline, N-methylaniline, N,N-dimethylaniline, and pyridine. These solvents can be used alone or in combination. Among these, ethanol, n-propanol, isopropanol, and tetrahydrofuran are particularly preferred from the viewpoints of solubility in the resin and ease of purification.

[0073] The acetalization is preferably carried out in the presence of an acid catalyst. The acid catalyst is not particularly limited, and examples thereof include mineral acids such as sulfuric acid, hydrochloric acid, nitric acid, and phosphoric acid, carboxylic acids such as formic acid, acetic acid, and propionic acid, and sulfonic acids such as methanesulfonic acid, ethanesulfonic acid, benzenesulfonic acid, and paratoluenesulfonic acid. These acid catalysts may be used alone or in combination of two or more compounds. Among these, hydrochloric acid, nitric acid, and sulfuric acid are preferred, and nitric acid is particularly preferred.

[0074] The acetalization is preferably carried out in the presence of the compound A. Specific examples of the compound A that can be used include compounds described below. By carrying out the acetalization in the presence of the compound A, a uniform acetalization reaction can be achieved.

[0075] The amount of compound A added is preferably 0.8 parts by weight or more, more preferably 1.2 parts by weight or more, and even more preferably 1.6 parts by weight or more, relative to 100 parts by weight of the polyvinyl alcohol resin, and is preferably 100 parts by weight or less, more preferably 50 parts by weight or less, and even more preferably 30 parts by weight or less. The amount added is preferably 0.8 to 100 parts by weight, more preferably 1.2 to 50 parts by weight, and even more preferably 1.6 to 30 parts by weight.

[0076] Examples of the aldehyde used in the acetalization include aldehydes having a chain aliphatic group, a cyclic aliphatic group, or an aromatic group having 1 to 10 carbon atoms. Conventionally known aldehydes can be used as these aldehydes. The aldehyde used in the acetalization reaction is not particularly limited, and examples include aliphatic aldehydes and aromatic aldehydes. Examples of the aliphatic aldehyde include formaldehyde, acetaldehyde, propionaldehyde, n-butyraldehyde, isobutyraldehyde, n-valeraldehyde, n-hexylaldehyde, 2-ethylbutyraldehyde, 2-ethylhexylaldehyde, n-heptylaldehyde, n-octylaldehyde, n-nonylaldehyde, n-decylaldehyde, and amylaldehyde. Examples of the aromatic aldehyde include benzaldehyde, cinnamaldehyde, 2-methylbenzaldehyde, 3-methylbenzaldehyde, 4-methylbenzaldehyde, p-hydroxybenzaldehyde, m-hydroxybenzaldehyde, phenylacetaldehyde, and β-phenylpropionaldehyde. These aldehydes may be used alone or in combination of two or more. Among these, preferred aldehydes are formaldehyde, acetaldehyde, butylaldehyde, 2-ethylhexylaldehyde, and n-nonylaldehyde, which have excellent acetalization reactivity and can provide a sufficient internal plasticizing effect to the resulting resin, thereby imparting good flexibility. Furthermore, formaldehyde, acetaldehyde, and butylaldehyde are more preferred because they can provide an adhesive composition that is particularly excellent in impact resistance and adhesion to metals.

[0077] The amount of the aldehyde to be added can be appropriately determined depending on the amount of acetal groups in the desired polyvinyl acetal resin.

[0078] The resin composition for a ceramic green sheet contains a compound A represented by the following formula (1): By containing the compound A, it is possible to reduce the amount of fine undissolved matter when the resin composition is dissolved in an organic solvent.

[0079]

[0080] In formula (1), R 1 and R 3 each independently represents a carboxyl group or a salt thereof, R 2 represents a single bond or a divalent group which may be substituted with at least one substituent selected from the group consisting of a hydroxyl group, a carboxyl group, and salts thereof. Examples of the salt include lithium salts, sodium salts, and potassium salts. 1 and R 3 may be the same or different, but are preferably the same. 2 is preferably a divalent group having at least one substituent selected from the group consisting of a hydroxyl group, a carboxyl group, and salts thereof.

[0081] The divalent group includes a divalent hydrocarbon group. Examples of the hydrocarbon group include a linear alkylene group having 1 to 6 carbon atoms, a branched alkylene group having 3 to 6 carbon atoms, a linear alkenylene group having 2 to 6 carbon atoms, a branched alkenylene group having 3 to 6 carbon atoms, a cycloalkylene group having 3 to 6 carbon atoms, a cycloalkenylene group having 3 to 6 carbon atoms, and an aromatic hydrocarbon group having 6 carbon atoms. Of these, a linear alkylene group having 1 to 4 carbon atoms and a branched alkylene group having 3 to 4 carbon atoms are preferred, and a linear alkylene group having 1 to 3 carbon atoms is more preferred.

[0082] Examples of the linear alkylene group having 1 to 6 carbon atoms include a methylene group, an ethylene group, a trimethylene group, a tetramethylene group, a pentamethylene group, and a hexamethylene group.

[0083] Examples of the branched alkylene group having 3 to 6 carbon atoms include a 1-methylethylene group, a 2-methyltrimethylene group, a 2-methyltetramethylene group, and a 2-methylpentamethylene group.

[0084] Examples of the linear alkenylene group having 2 to 6 carbon atoms include a vinylene group, a propenylene group, a butenylene group, and a hexenylene group.

[0085] Examples of branched alkenylene groups having 3 to 6 carbon atoms include an isopropenylene group, a 1-ethylethenylene group, a 2-methylpropenylene group, a 2,2-dimethylbutenylene group, a 3-methyl-2-butenylene group, and a 3-ethyl-2-butenylene group.

[0086] Examples of the cycloalkylene group having 3 to 6 carbon atoms include a cyclopentylene group and a cyclohexylene group.

[0087] Examples of the cycloalkenylene group having 3 to 6 carbon atoms include a cyclopentenylene group, a 2,4-cyclopentadienylene group, and a cyclohexenylene group.

[0088] Examples of aromatic hydrocarbon groups having 6 carbon atoms include 1,2-phenylene.

[0089] R 2 More specifically, preferred examples of the alkyl group include a hydroxyethylene group, a 1,2-dihydroxyethylene group, a 2-hydroxy, 2-carboxytrimethylene group, a hydroxymethylene group, a trimethylene group, and a methylene group, and more preferred examples are a hydroxyethylene group, a 1,2-dihydroxyethylene group, and a 2-hydroxy, 2-carboxytrimethylene group.

[0090] The molecular weight of the compound A is preferably 90 or more, more preferably 130 or more, and even more preferably 150 or more, and is preferably 10,000 or less, more preferably 1,000 or less, and even more preferably 500 or less. The molecular weight is preferably 90 to 10,000, more preferably 130 to 1,000, and even more preferably 150 to 500.

[0091] Specific examples of the compound A include aliphatic hydroxy acids such as citric acid, malic acid, tartaric acid, tartronic acid, isocitric acid, and mevalonic acid, and aliphatic dicarboxylic acids such as oxalic acid, malonic acid, fumaric acid, succinic acid, glutaric acid, adipic acid, and suberic acid. Of these, citric acid, malic acid, tartaric acid, tartronic acid, glutaric acid, and malonic acid are preferred, and citric acid, malic acid, and tartaric acid are more preferred.

[0092] The content of Compound A in the resin composition for ceramic green sheets is 2 ppm or more by weight, since this can improve solubility in organic solvents. The content of Compound A is preferably 5 ppm or more by weight, more preferably 10 ppm or more, and is preferably 29,000 ppm or less, more preferably 28,000 ppm or less, and even more preferably 26,000 ppm or less. The content is preferably 2 to 29,000 ppm, more preferably 5 to 28,000 ppm, and even more preferably 10 to 26,000 ppm. The content of Compound A can be measured, for example, by ion chromatography.

[0093] The content of Compound A in the resin composition for a ceramic green sheet is preferably 2 ppm or more, more preferably 5 ppm or more, and even more preferably 10 ppm or more, and is preferably 29,000 ppm or less, more preferably 28,000 ppm or less, and even more preferably 26,000 ppm or less, relative to 100 parts by weight of the polyvinyl acetal resin. The content is preferably 2 to 29,000 ppm, more preferably 5 to 28,000 ppm, and even more preferably 10 to 26,000 ppm.

[0094] In the resin composition for ceramic green sheets, X, represented by the following formula (2), is preferably 1.6 or more and preferably 4.5 or less. By setting it within this range, uniform solvent solubility is ensured and mechanical strength can be improved. X is more preferably 1.7 or more and more preferably 4.4 or less. X is preferably 1.6 to 4.5, more preferably 1.7 to 4.4.

[0095]

[0096] The resin composition for a ceramic green sheet may contain components such as an antioxidant, an ultraviolet absorber, a surfactant, and a defoamer, as long as the effects of the present invention are not impaired.

[0097] As a method for producing the resin composition for ceramic green sheets, for example, a polyvinyl alcohol resin can be acetalized with an aldehyde in the presence of the compound A to obtain a resin composition for ceramic green sheets containing a polyvinyl acetal resin and the compound A. Alternatively, for example, the compound A and other additives added as needed can be added to and mixed with a polyvinyl acetal resin obtained by acetalizing a polyvinyl alcohol resin with an aldehyde to obtain a resin composition for ceramic green sheets.

[0098] The resin composition for a ceramic green sheet, an organic solvent, and inorganic fine particles are mixed together to prepare an inorganic fine particle dispersion slurry composition.

[0099] The organic solvent is not particularly limited as long as it can dissolve the polyvinyl acetal resin, and examples thereof include ketones such as acetone, methyl ethyl ketone, dipropyl ketone, and diisobutyl ketone. Other examples include alcohols such as methanol, ethanol, isopropanol, and butanol, and aromatic hydrocarbons such as toluene and xylene. Further examples include esters such as methyl propionate, ethyl propionate, butyl propionate, methyl butanoate, ethyl butanoate, butyl butanoate, methyl pentanoate, ethyl pentanoate, butyl pentanoate, methyl hexanoate, ethyl hexanoate, butyl hexanoate, 2-ethylhexyl acetate, and 2-ethylhexyl butyrate. Other examples include methyl cellosolve, ethyl cellosolve, butyl cellosolve, terpineol, dihydroterpineol, butyl cellosolve acetate, butyl carbitol acetate, terpineol acetate, and dihydroterpineol acetate. In particular, alcohols, ketones, aromatic hydrocarbons and mixed solvents thereof are preferred in terms of coating and drying properties, with a mixed solvent of ethanol and toluene and a mixed solvent of methyl ethyl ketone and toluene being more preferred.

[0100] The content of the organic solvent in the inorganic fine particle dispersion slurry composition is determined depending on the type of polyvinyl acetal resin used and is not particularly limited, but if the content is too low, the solubility required for kneading is difficult to exhibit. On the other hand, if the content is too high, the viscosity of the slurry composition becomes too low, which may result in poor handling when producing ceramic green sheets. Therefore, the content of the organic solvent is preferably 20% by weight or more and 80% by weight or less.

[0101] The inorganic fine particle dispersion slurry composition contains inorganic fine particles, and the inorganic fine particles are not particularly limited, and examples thereof include ceramic powder, glass powder, and metal fine particles.

[0102] The ceramic powder is not particularly limited, and examples thereof include powders of metal or nonmetal oxides, carbides, nitrides, borides, sulfides, etc. used in ceramic production. Specific examples include oxides, carbides, nitrides, borides, sulfides, etc. of Li, K, Mg, B, Al, Si, Cu, Ca, Sr, Ba, Zn, Cd, Ga, In, Y, lanthanides, actinides, Ti, Zr, Hf, Bi, V, Nb, Ta, W, Mn, Fe, Co, Ni, etc. These ceramic powders may be used alone or as a mixture of two or more types. Examples of such materials include barium titanate, aluminum nitride (AlN), silicon nitride (Si3N4), silicon carbide (SiC), alumina (Al2O3), copper oxide (CuO), and spinel compounds, ferrite, zirconia, zircon, barium zirconate, calcium zirconate, titanium oxide, barium titanate, strontium titanate, calcium titanate, magnesium titanate, zinc titanate, lanthanum titanate, neodymium titanate, lead zirconate titanate, alumina nitride, silicon nitride, boron nitride, boron carbide, barium stannate, calcium stannate, magnesium silicate, mullite, steatite, cordierite, and forsterite.

[0103] The glass powder is not particularly limited, and examples thereof include glass powders such as bismuth oxide glass, silicate glass, lead glass, zinc glass, and boron glass, and CaO—Al 2 O 3-SiO 2 system, MgO-Al 2 O 3 -SiO 2 system, LiO 2 -Al 2 O 3 -SiO 2 Examples of the glass powder include glass powders of various silicon oxides such as SnO—B 2 O 3 -P 2 O 5 -Al 2 O 3 mixture, PbO-B 2 O 3 -SiO 2 Mixture, BaO-ZnO-B 2 O 3 -SiO 2 Mixture, ZnO-Bi 2 O 3 -B 2 O 3 -SiO 2 mixture, Bi 2 O 3 -B 2 O 3 -BaO-CuO mixture, Bi 2 O 3 -ZnO-B 2 O 3 -Al 2 O 3 -SrO mixture, ZnO-Bi 2 O 3 -B 2 O 3 mixture, Bi 2 O 3 -SiO 2 mixture, P 2 O 5 -Na 2 O-CaO-BaO-Al 2 O 3 -B 2 O 3 mixture, P 2 O 5 -SnO mixture, P 2 O 5 -SnO-B 2 O 3 mixture, P 2 O 5 -SnO-SiO2 mixture, CuO-P 2 O 5 -RO mixture, SiO 2 -B 2 O 3 -ZnO-Na 2 O-Li 2 O-NaF-V 2 O 5 mixture, P 2 O 5 -ZnO-SnO-R 2 O-RO mixture, B 2 O 3 -SiO 2 -ZnO mixture, B 2 O 3 -SiO 2 -Al 2 O 3 -ZrO 2 mixture, SiO 2 -B 2 O 3 -ZnO-R 2 O-RO mixture, SiO 2 -B 2 O 3 -Al 2 O 3 -RO-R 2 O mixture, SrO-ZnO-P 2 O 5 Mixture, SrO-ZnO-P 2 O 5 Mixture, BaO-ZnO-B 2 O 3 -SiO 2 A mixture of these elements can also be used. R is an element selected from the group consisting of Zn, Ba, Ca, Mg, Sr, Sn, Ni, Fe, and Mn. In particular, PbO—B 2 O 3 -SiO 2 Mixture glass powder and lead-free BaO-ZnO-B 2 O 3 -SiO 2 Mixture or ZnO-Bi 2 O 3 -B 2 O 3 -SiO 2 Lead-free glass powders such as mixtures are preferred.

[0104] The metal particles are not particularly limited, and examples thereof include powders of copper, nickel, palladium, iron, platinum, gold, silver, aluminum, tungsten, and alloys thereof. In addition to metal complexes, various carbon blacks, carbon nanotubes, and the like may also be used. Other usable materials include ITO, FTO, niobium oxide, vanadium oxide, tungsten oxide, lanthanum strontium manganite, lanthanum strontium cobalt ferrite, yttrium-stabilized zirconia, gadolinium-doped ceria, nickel oxide, and lanthanum chromite.

[0105] The content of the inorganic fine particles in the inorganic fine particle dispersion slurry composition is not particularly limited, but is preferably 10% by weight or more, more preferably 15% by weight or more, and is preferably 90% by weight or less, and more preferably 85% by weight or less. By setting the content within the above range, the composition can have sufficient viscosity and excellent coatability, and can also have excellent dispersibility of the inorganic fine particles. The content is preferably 10 to 90% by weight, more preferably 15 to 85% by weight.

[0106] The inorganic fine particle dispersion slurry composition contains a plasticizer. Examples of the plasticizer include monomethyl adipate, di(butoxyethyl adipate), dibutoxyethoxyethyl adipate, triethylene glycol bis(2-ethylhexanoate), triethylene glycol dihexanoate, triethyl acetylcitrate, tributyl cetyl citrate, dibutyl sebacate, butylated benzyl phthalate, diisononyl adipate, diisodecyl phthalate, tripropionin, pentaerythritol tetraacetate, di-2-ethylhexyl phthalate, and triacetin. Among these, triethylene glycol bis(2-ethylhexanoate), butylated benzyl phthalate, diisononyl adipate, diisodecyl phthalate, tripropionin, pentaerythritol tetraacetate, and di-2-ethylhexyl phthalate are preferred.

[0107] The boiling point of the plasticizer is preferably 240°C or higher, and preferably lower than 390°C. By setting the boiling point to 240°C or higher, the plasticizer is easily evaporated in the drying step, and it is possible to prevent the plasticizer from remaining in the molded body. Furthermore, by setting the boiling point to lower than 390°C, it is possible to prevent the formation of residual carbon. The boiling point is preferably 240°C or higher but lower than 390°C. The boiling point refers to the boiling point at normal pressure.

[0108] The content of the plasticizer in the inorganic fine particle dispersion slurry composition is not particularly limited, but is preferably 0.1 wt% or more, more preferably 0.2 wt% or more, and preferably 3 wt% or less, and more preferably 2.5 wt% or less. By keeping the content within this range, the calcination residue of the plasticizer can be reduced. The content is preferably 0.1 to 3 wt%, more preferably 0.2 to 2.5 wt%.

[0109] The viscosity of the inorganic fine particle dispersion slurry composition is not particularly limited, but when measured at 20°C using a Brookfield viscometer with the probe rotation speed set to 5 rpm, the viscosity is preferably 0.1 Pa·s or more and preferably 100 Pa·s or less. The viscosity is preferably 0.1 to 100 Pa·s. By setting the viscosity to 0.1 Pa·s or more, it becomes possible for the resulting inorganic fine particle dispersion sheet to maintain a predetermined shape after coating by a die coat printing method or the like. Furthermore, by setting the viscosity to 100 Pa·s or less, defects such as indelible die coating marks can be prevented, and excellent printability can be achieved.

[0110] The method for preparing the inorganic fine particle dispersion slurry composition is not particularly limited, and examples thereof include conventionally known stirring methods. Specific examples thereof include a method of stirring the resin composition for ceramic green sheets, the inorganic fine particles, an organic solvent added as needed, a plasticizer, and other components using a bead mill or the like.

[0111] The inorganic fine particle dispersion slurry composition is applied to a support film that has been subjected to a release treatment on one side, the organic solvent is dried, and the film is formed into a sheet, thereby producing an inorganic fine particle dispersion sheet. The inorganic fine particle dispersion sheet preferably has a thickness of 0.5 μm or more and 3 μm or less.

[0112] The support film used in producing the inorganic fine particle-dispersed sheet is preferably a resin film having heat resistance, solvent resistance, and flexibility. The flexibility of the support film allows the inorganic fine particle-dispersed slurry composition to be applied to the surface of the support film using a roll coater, blade coater, or the like, and the resulting inorganic fine particle-dispersed sheet-forming film to be stored and supplied in a rolled state.

[0113] Examples of resins that form the support film include fluorine-containing resins such as polyethylene terephthalate, polyester, polyethylene, polypropylene, polystyrene, polyimide, polyvinyl alcohol, polyvinyl chloride, and polyfluoroethylene, nylon, and cellulose. The thickness of the support film is preferably, for example, 20 μm or more and 100 μm or less. The surface of the support film is preferably subjected to a release treatment, which allows the support film to be easily peeled off in the transfer step.

[0114] Furthermore, the inorganic fine particle dispersed slurry composition and the inorganic fine particle dispersed sheet can be used for a dielectric green sheet and an electrode paste to produce a multilayer ceramic capacitor.

[0115] The method for producing the multilayer ceramic capacitor preferably includes the steps of printing and drying a conductive paste on the inorganic fine particle dispersed sheet to produce a dielectric sheet, and laminating the dielectric sheets.

[0116] The conductive paste contains a conductive powder. The material of the conductive powder is not particularly limited as long as it is a conductive material, and examples thereof include nickel, palladium, platinum, gold, silver, copper, and alloys thereof. These conductive powders may be used alone or in combination of two or more.

[0117] The binder resin and organic solvent used in the conductive paste may be the same as those used in the inorganic fine particle dispersion slurry composition.

[0118] The method for printing the conductive paste is not particularly limited, and examples thereof include screen printing, die coating printing, offset printing, gravure printing, and inkjet printing.

[0119] In the method for producing the multilayer ceramic capacitor, the dielectric sheets on which the conductive paste is printed are laminated, degreased, fired, and then external electrodes are provided to obtain the multilayer ceramic capacitor.

[0120] According to the present invention, it is possible to provide a resin composition for ceramic green sheets which has excellent solvent solubility and which, when dissolved in an organic solvent, reduces the amount of fine undissolved matter and enables the production of highly reliable ceramic capacitors.

[0121] The present invention will be explained in more detail below with reference to examples, but the present invention is not limited to these examples.

[0122] Example 1 200 g of polyvinyl alcohol resin (average polymerization degree 3,300, saponification degree 99 mol%, purity 96.5%) was added to 2300 g of pure water and dissolved by stirring at 90°C for 2 hours. This solution was cooled to 40°C, and 181 g of 35 wt% hydrochloric acid, 3.1 g of malic acid, and 116 g of n-butyl aldehyde were added to carry out an acetalization reaction, resulting in the precipitation of the reaction product. The mixture was then held at 40°C for 3 hours to complete the reaction, and neutralized, washed with water, and dried by conventional methods to obtain a resin composition for ceramic green sheets containing polyvinyl acetal resin and malic acid. The resulting polyvinyl acetal resin was dissolved in DMSO-D 6 (dimethyl sulfoxide), 1Analysis using H-NMR (nuclear magnetic resonance spectroscopy) revealed that the amounts of acetal groups, acetyl groups, and hydroxyl groups were as shown in Table 1. Furthermore, the content of malic acid in the resin composition for ceramic green sheets was confirmed by ion chromatography, and was found to be 2.9 ppm by weight. The measuring instrument used was an ion chromatography system ICS900 (manufactured by Thermo Fisher Scientific, column: Ionpac AS22 (4φ×250 mm), detector: electrical conductivity meter). Furthermore, the value of X was calculated according to the following formula (2).

[0123]

[0124] Example 2 A resin composition for a ceramic green sheet was obtained in the same manner as in Example 1, except that tartaric acid was used instead of malic acid.

[0125] Example 3 A resin composition for a ceramic green sheet was obtained in the same manner as in Example 1, except that 30.9 g of citric acid was used instead of malic acid.

[0126] Example 4 A resin composition for ceramic green sheets was obtained in the same manner as in Example 1, except that the amount of n-butylaldehyde added was 110 g.

[0127] Example 5 A resin composition for a ceramic green sheet was obtained in the same manner as in Example 1, except that tartronic acid was used instead of malic acid.

[0128] Example 6 A resin composition for a ceramic green sheet was obtained in the same manner as in Example 1, except that glutaric acid was used instead of malic acid.

[0129] Example 7 A resin composition for a ceramic green sheet was obtained in the same manner as in Example 1, except that 6.2 g of malonic acid was used instead of malic acid.

[0130] Example 8: 200 g of polyvinyl alcohol resin (average polymerization degree 3,300, saponification degree 99 mol%, purity 96.5%) was added to 2300 g of pure water and stirred at 90°C for 2 hours to dissolve. This solution was cooled to 40°C, and 181 g of 35 wt% hydrochloric acid, 3.1 g of malic acid, and 116 g of n-butyl aldehyde were added to carry out an acetalization reaction, resulting in precipitation of the reaction product. The mixture was then held at 40°C for 3 hours to complete the reaction. The mixture was then neutralized and washed with water by conventional methods and adjusted to a volatile content of 50 wt% in a centrifugal dehydrator. Next, 2830 g of pure water and 38.0 g of malic acid were added, stirred for 1 hour, and then adjusted to a volatile content of 50 wt% in a centrifugal dehydrator. The mixture was then dried to obtain a resin composition for ceramic green sheets containing polyvinyl acetal resin and malic acid.

[0131] Example 9: 200 g of polyvinyl alcohol resin (average degree of polymerization: 3,300, degree of saponification: 82 mol%, purity: 96.5%) was added to 2300 g of pure water and stirred at 90°C for 2 hours to dissolve. This solution was cooled to 40°C, and 181 g of 35 wt% hydrochloric acid, 3.1 g of malic acid, and 127 g of n-butyl aldehyde were added to carry out an acetalization reaction, resulting in precipitation of the reaction product. The mixture was then held at 40°C for 3 hours to complete the reaction. The mixture was then neutralized and washed with water by conventional methods and adjusted to a volatile content of 50 wt% in a centrifugal dehydrator. Next, 2640 g of pure water and 76.0 g of malic acid were added, stirred for 1 hour, and then adjusted to a volatile content of 50 wt% in a centrifugal dehydrator. The mixture was then dried to obtain a resin composition for ceramic green sheets containing polyvinyl acetal resin and malic acid.

[0132] Comparative Example 1 A resin composition for a ceramic green sheet was obtained in the same manner as in Example 1, except that malic acid was not added.

[0133] Comparative Example 2 A resin composition for a ceramic green sheet was obtained in the same manner as in Example 1, except that a polyvinyl alcohol resin (average degree of polymerization 3,300, degree of saponification 99.2 mol%, purity 96.5%) was used, the amount of n-butyl aldehyde added was 117 g, and malic acid was not added.

[0134] Comparative Example 3 A resin composition for a ceramic green sheet was obtained in the same manner as in Example 1, except that 3.1 g of pentaerythritol was used instead of malic acid.

[0135] Comparative Example 4: 200 g of polyvinyl alcohol resin (average polymerization degree 3,300, saponification degree 78 mol%, purity 96.5%) was added to 2300 g of pure water and stirred at 90°C for 2 hours to dissolve. This solution was cooled to 40°C, and 181 g of 35 wt% hydrochloric acid and 133 g of n-butyl aldehyde were added to carry out an acetalization reaction, resulting in precipitation of the reaction product. The mixture was then held at 40°C for 3 hours to complete the reaction. The mixture was then neutralized and washed with water in a conventional manner, and the volatile content was adjusted to 50 wt% in a centrifugal dehydrator. Next, 2590 g of pure water and 132.8 g of pentaerythritol were added, stirred for 1 hour, and then adjusted to 50 wt% in a centrifugal dehydrator. The resulting mixture was then dried to obtain a resin composition for ceramic green sheets containing polyvinyl acetal resin and pentaerythritol.

[0136] Example 10 A resin composition for ceramic green sheets was obtained in the same manner as in Example 1, except that a polyvinyl alcohol resin (average degree of polymerization: 1,700, degree of saponification: 99 mol %) was used.

[0137] Example 11 A resin composition for a ceramic green sheet was obtained in the same manner as in Example 10, except that 6.2 g of tartaric acid was used instead of malic acid.

[0138] Example 12 A resin composition for a ceramic green sheet was obtained in the same manner as in Example 10, except that the amount of malic acid added was changed to 12.4 g.

[0139] Comparative Example 5 A resin composition for a ceramic green sheet was obtained in the same manner as in Example 10, except that malic acid was not added.

[0140] Comparative Example 6 A resin composition for a ceramic green sheet was obtained in the same manner as in Example 10, except that the amount of tartaric acid added was changed to 1.5 g.

[0141] Example 13: 200 g of polyvinyl alcohol resin (average polymerization degree 700, saponification degree 98.5 mol%) was added to 2300 g of pure water and stirred at 90°C for 2 hours to dissolve. This solution was cooled to 40°C, and 181 g of 35 wt% hydrochloric acid, 3.1 g of tartaric acid, and 116 g of n-butyl aldehyde were added to carry out an acetalization reaction, resulting in precipitation of the reaction product. The mixture was then held at 40°C for 3 hours to complete the reaction. The mixture was then neutralized and washed with water by conventional methods, and the volatile content was adjusted to 35 wt% in a centrifugal dehydrator. Next, 1630 g of pure water was added, and the mixture was stirred for 1 hour. The polyvinyl acetal resin concentration was then adjusted to 12 wt% in a centrifugal dehydrator, followed by drying to obtain a resin composition for ceramic green sheets containing the polyvinyl acetal resin and tartaric acid.

[0142] Example 14 A resin composition for ceramic green sheets was obtained in the same manner as in Example 1, except that a polyvinyl alcohol resin (average polymerization degree 700, saponification degree 98.5 mol%) was used and 6.2 g of tartaric acid was used instead of malic acid.

[0143] Example 15 A resin composition for a ceramic green sheet was obtained in the same manner as in Example 14, except that the amount of tartaric acid added was changed to 12.4 g.

[0144] Comparative Example 7 A resin composition for ceramic green sheets was obtained in the same manner as in Example 14, except that a polyvinyl alcohol resin (average polymerization degree 700, saponification degree 99 mol %) was used and tartaric acid was not added.

[0145] <Evaluation> The obtained polyvinyl acetal resin and resin composition for ceramic green sheet were evaluated as follows. The results are shown in Table 1.

[0146] (1) Porosity The porosity of the obtained polyvinyl acetal resin was measured by mercury intrusion porosimetry using a porosimeter (Thermo Pascal 14B). The porosity refers to the volume of pores with a pore radius of 0.0038 to 7.5 μm relative to the volume of the resin particles.

[0147] (2) Particle Diameter (D50) The particle diameter (D50) of the obtained polyvinyl acetal resin was measured using a laser diffraction particle size distribution measuring device (Mastersizer 3000).

[0148] (3) Dissolution Time: 192 g of a mixed solvent of ethanol and toluene (weight ratio 1:1) was placed in a 500 mL beaker. The temperature was maintained at 25°C. While stirring at 200 rpm using two stirring blades, 48.0 g (6 wt % concentration of the resin composition) of the polyvinyl acetal resin compositions obtained in Examples 1 to 9 and Comparative Examples 1 to 4 (average resin polymerization degree 3300) was added to dissolve the polyvinyl acetal resin composition. Visual observation was performed to measure the dissolution time from the addition of the resulting polyvinyl acetal resin composition until no undissolved resin remained. Similarly, the dissolution time was measured at a concentration of 10 wt % for the polyvinyl acetal resin compositions obtained in Examples 10 to 12 and Comparative Examples 5 and 6 (average resin polymerization degree 1700), and at a concentration of 20 wt % for the polyvinyl acetal resin compositions obtained in Examples 13 to 15 and Comparative Example 7 (average resin polymerization degree 700).

[0149] (4) Dissolution Time Reduction Rate For Examples 1 to 9 and Comparative Examples 2 to 4, the dissolution time reduction rate (%) was calculated using the dissolution time of Comparative Example 1 as the reference. For Examples 10 to 12 and Comparative Example 6, the dissolution time reduction rate (%) was calculated using the dissolution time of Comparative Example 5 as the reference. Furthermore, for Examples 13 to 15, the dissolution time reduction rate (%) was calculated using the dissolution time of Comparative Example 7 as the reference. Specifically, the dissolution time reduction rate (%) was calculated according to the following formula: Dissolution time reduction rate (%) = [(reference dissolution time - dissolution time of each example) / reference dissolution time] x 100

[0150] (5) Number of particles with a particle diameter of 0.5 to 1.0 μm The obtained resin composition for a ceramic green sheet was dissolved in a mixed solution of ethanol and toluene at a weight ratio of 1:1 so as to have a concentration of 0.2 wt %. The particle size distribution of 10 ml of the obtained solution was measured using a particle counter (KS-42C, manufactured by Rion Co., Ltd.), and the number of particles with a diameter of 0.5 to 1.0 μm per 10 ml was measured.

[0151] (6) Evaluation of Ceramic Green Sheets (Preparation of Inorganic Dispersion) 1 part by weight of polyvinyl acetal resin (BL-1, manufactured by Sekisui Chemical Co., Ltd.) was added to a mixed solvent of 20 parts by weight of toluene and 20 parts by weight of ethanol, and dissolved by stirring. Next, 100 parts by weight of barium titanate powder (BT01, manufactured by Sakai Chemical Industry Co., Ltd.) was added to the obtained solution, and the mixture was stirred for 180 minutes using a bead mill (Ready Mill, manufactured by Imex Co., Ltd.) to prepare an inorganic dispersion.

[0152] (Preparation of Resin Solutions) For Examples 1 to 9 and Comparative Examples 1 to 4, the resulting ceramic green sheet resin composition was dissolved in a mixed solvent of ethanol and toluene (weight ratio 1:1) to prepare a resin composition solution with a resin composition concentration of 6 wt %. To 98 parts by weight of the resulting resin composition solution, 2 parts by weight of dioctyl phthalate (DOP) was added and stirred to dissolve, thereby preparing a resin solution. For Examples 10 to 12 and Comparative Examples 5 and 6, the resulting ceramic green sheet resin composition was dissolved in a mixed solvent of ethanol and toluene (weight ratio 1:1) to prepare a resin composition solution with a resin composition concentration of 8 wt %. To 98 parts by weight of the resulting resin composition solution, 2 parts by weight of DOP was added and stirred to dissolve, thereby preparing a resin solution. Furthermore, for Examples 13 to 15 and Comparative Example 7, the resulting ceramic green sheet resin composition was dissolved in a mixed solvent of ethanol and toluene (weight ratio 1:1) to prepare a resin composition solution with a resin composition concentration of 15 wt %. To 98 parts by weight of the obtained resin composition solution, 2 parts by weight of DOP was added and dissolved by stirring to prepare a resin solution.

[0153] (Preparation of ceramic green sheets) The resin solution was added to the inorganic dispersion and stirred for 90 minutes in a bead mill to obtain a ceramic green sheet composition. The obtained ceramic green sheet composition was applied to a release-treated PET film using a coater so that the thickness after drying would be 20 μm, and then heated and dried to prepare a ceramic green sheet.

[0154] (6-1) Cross-sectional area 1 μm 2The number of defects on the surface of the obtained ceramic green sheet is 14,000 μm or more. 2 Ten visual fields were randomly selected, and the average number of defects per visual field was counted using a shape analysis laser microscope (Keyence Corporation, "VK-X100"). The defects were defined as protruding valleys with a cross-sectional area of ​​1 μm when the areal load ratio was 80%. 2 The above is the part.

[0155] (6-2) Arithmetic Mean Height (Sa) and Maximum Height (Sz) The arithmetic mean height Sa of the obtained ceramic green sheet was evaluated in accordance with ISO 25178 using a three-dimensional surface roughness meter (VertScan 2.0 manufactured by Ryoka Systems Co., Ltd.).

[0156]

[0157]

[0158]

[0159] According to the present invention, it is possible to provide a resin composition for ceramic green sheets which has excellent solvent solubility and which, when dissolved in an organic solvent, reduces the amount of fine undissolved matter and enables the production of highly reliable ceramic capacitors.

Claims

1. The composition contains a polyvinyl acetal resin and a compound A represented by the following formula (1): The resin composition for ceramic green sheets, wherein the content of the compound A is 2 ppm or more by weight. 【Chemistry 1】 In formula (1), R 1 and R 3 each independently represents a carboxyl group or a salt thereof; R 2 represents a single bond or a divalent group which may be substituted with at least one substituent selected from the group consisting of a hydroxyl group, a carboxyl group, and salts thereof.

2. In formula (1), R 2 is a linear alkylene group having 1 to 6 carbon atoms which may be substituted with at least one substituent selected from the group consisting of a hydroxyl group, a carboxyl group, and salts thereof.

3. In formula (1), R 2 3. The resin composition for a ceramic green sheet according to claim 1, wherein is a linear alkylene group having 1 to 3 carbon atoms and having at least one group selected from the group consisting of a hydroxyl group, a carboxyl group, and salts thereof.

4. 3. The resin composition for a ceramic green sheet according to claim 1, wherein X represented by the following formula (2) is 1.6 or more and 4.5 or less: [0010]

5. 3. The resin composition for a ceramic green sheet according to claim 1, wherein compound A is at least one compound selected from the group consisting of tartaric acid, malic acid, citric acid, and salts thereof.

6. 3. The resin composition for ceramic green sheets according to claim 1, wherein the polyvinyl acetal resin has a solution viscosity of 50 mPa·s or more at 20° C. when dissolved in an ethanol / toluene mixed solution (weight ratio 1:1) at 10% by weight.

7. 3. The resin composition for a ceramic green sheet according to claim 1, wherein the polyvinyl acetal resin has an acetyl group content of 0.5% by weight or more and 20% by weight or less.

8. 3. The resin composition for a ceramic green sheet according to claim 1, wherein the polyvinyl acetal resin has an average degree of polymerization of 500 or more.