Method for producing group 13 element nitride crystal substrate

JPWO2023277103A5Active Publication Date: 2024-11-08KYOCERA CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023532039
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-06-29
Filing Date
2022-06-29
Publication Date
2024-11-08
Estimated Expiration
2042-06-29

AI Technical Summary

Technical Problem

Conventional gallium nitride (GaN) single crystal substrates with polar surfaces suffer from reduced luminous efficiency due to internal electric fields, and their anisotropic workability complicates processing, particularly between Ga-face and N-face surfaces, limiting the performance of light-emitting devices.

Method used

A method involving grinding and chemical mechanical polishing (CMP) processes using a carbon fiber reinforced plastic (CFRP) carrier to manufacture substrates with semipolar or nonpolar surfaces, which reduces polarity-related issues and improves workability, involving specific orientations and slurry compositions to enhance surface quality and productivity.

Benefits of technology

The method improves the luminous efficiency and workability of GaN substrates by reducing internal electric fields and anisotropy, leading to higher-quality substrates suitable for high-efficiency light-emitting devices with reduced manufacturing costs and increased productivity.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

A production method according to the present disclosure comprises: a grinding step in which a group 13 element nitride crystal is contained in an opening of a plate-like carrier, and at least one main surface of the crystal is ground; and a CMP step in which the main surface after grinding is subjected to chemical mechanical polishing (CMP), while keeping the substrate contained in the carrier. The main surface is a semi-polar surface, a non-polar or an N surface; the slurry used in the CMP step is alkaline; and the carrier is formed of a carbon fiber reinforced plastic.
Need to check novelty before this filing date? Find Prior Art

Description

Method for manufacturing a nitride crystal substrate of group 13 elements of the periodic table

[0001] The present disclosure relates to a method for manufacturing a crystal substrate of a nitride of a Group 13 element of the periodic table, such as a gallium nitride (GaN) single crystal substrate.

[0002] Periodic table Group 13 element nitride crystals (hereinafter sometimes simply referred to as Group 13 element nitride crystals), typified by gallium nitride (GaN), have excellent semiconductor properties such as band gap and breakdown field, and are therefore useful materials for light-emitting devices such as light-emitting diodes and laser diodes, as well as high-frequency and high-power electronic devices.

[0003] Group 13 element nitride crystals have a hexagonal crystal structure and are polar in the c-axis direction. Conventionally, gallium nitride single crystals with polar (c-plane) main surfaces have been used in gallium nitride-based light-emitting diodes (LEDs). However, a phenomenon known as droop, in which electrons and holes are separated by an internal electric field due to polarity, resulting in a decrease in light-emitting efficiency, has been reported. Therefore, development of devices such as LEDs using gallium nitride crystals with semipolar or nonpolar main surfaces is progressing. Furthermore, gallium nitride single crystals have anisotropy in processability due to polarity, with the processability differing between the Ga and N faces of c-plane gallium nitride crystals.

[0004] Gallium nitride single crystal processing mainly includes grinding and chemical mechanical polishing (hereinafter referred to as CMP) processing (polishing). Patent documents 1 and 2 describe grinding of gallium nitride single crystal substrates. Patent document 3 also describes polishing the N-face side of a c-plane gallium nitride single crystal substrate with an alkaline CMP slurry and the Ga-face side with an acidic CMP slurry. Patent document 3 also describes mounting a substrate on a template having a recess or a flat template and lapping or polishing it.

[0005] JP 2013-211491 A JP 2013-229586 A JP 2009-164634 A

[0006] The presently disclosed method for manufacturing a Group 13 element nitride crystal substrate comprises a grinding step in which a Group 13 element nitride crystal is placed in an opening in a plate-shaped carrier and at least one of the crystal's main surfaces is ground, and a CMP step in which the ground main surface is subjected to CMP while the substrate is still placed in the carrier. The main surface is a semi-polar, non-polar, or N-face, the slurry used in the CMP step is alkaline, and the carrier is made of carbon fiber reinforced plastic (CFRP).

[0007] 5A is a flowchart showing the steps of a method for manufacturing a Group 13 element nitride crystal substrate according to an embodiment of the present disclosure.

[0023] FIG. 5B is a schematic diagram illustrating a polar face of a gallium nitride single crystal, which is a Group 13 element nitride crystal.

[0024] FIG. 5C is a schematic diagram illustrating a semi-polar face of a gallium nitride single crystal, which is a Group 13 element nitride crystal.

[0025] FIG. 5D is a schematic diagram illustrating a non-polar face of a gallium nitride single crystal, which is a Group 13 element nitride crystal.

[0026] FIG. 5E is a schematic diagram illustrating a grinding process for a gallium nitride single crystal.

[0027] FIG. 5F is a plan view showing an example of a carrier according to the present disclosure.

[0028] FIG. 5G is a plan view showing a schematic representation of the positional relationship between a single crystal holder and a wheel-shaped grindstone holder in a surface grinding process.

[0029] FIG. 5H is a partial side view of FIG. 5A.

[0030] FIG. 5H is an explanatory diagram showing the relationship between the gap between adjacent gallium nitride single crystals and the width of the grindstone track in a grinding process.

[0031] FIG. 5I is an explanatory diagram showing the relationship between the gallium nitride single crystal and the grindstone track in a grinding process.

[0032] FIG. 5I is an explanatory diagram showing the relationship between the gallium nitride single crystal and the grindstone track in a grinding process.

[0033] FIG. 5I is an explanatory diagram showing the relationship between the gallium nitride single crystal and the grindstone track in a grinding process.

[0034] FIG. 5I is an explanatory diagram showing the relationship between the gallium nitride single crystal and the grindstone track in a grinding process.

[0035] FIG. 5I is an explanatory diagram showing the relationship between the gallium nitride single crystal and the grindstone track in a grinding process.

[0036] 16A is a schematic cross-sectional view of portion C1 of FIG. 8B , showing the grinding wheel trajectory including portions b1 and b2. FIG. 16B is a schematic cross-sectional view of portion C2 of FIG. 8B , showing the grinding wheel trajectory 8'. FIG. 16B is an explanatory view showing an example of an attached state of a plurality of gallium nitride single crystals. FIG. 16A is a schematic view for explaining the definition of the range of angles for grinding in the surface grinding process. FIG. 16B is an explanatory view showing the ranges A to F of angles for grinding in the surface grinding process. FIG. 16B is a schematic view showing the CMP process for a gallium nitride single crystal. FIG. 16A is a graph showing the difference in thickness between the carrier and the single crystal after polishing in the CMP process. FIG. 16B is an explanatory view for explaining face sagging of a single crystal during polishing in the CMP process. FIG. 16B is an explanatory view for explaining face sagging of a single crystal during polishing in the CMP process. FIG. 16B is an explanatory view for explaining face sagging of a single crystal during polishing in the CMP process. FIG. 16A is an explanatory view for explaining face sagging of a single crystal during polishing in the CMP process. FIG. 16B is an explanatory view for explaining face sagging of a single crystal during polishing in the CMP process. FIG. 16B is an explanatory view for explaining face sagging of a single crystal during polishing in the CMP process. FIG. 16B is a plan view showing a carrier. FIG. 16A is an enlarged view of portion M of FIG.

[0008] Hereinafter, the method for manufacturing a Group 13 element nitride single crystal substrate according to the present disclosure will be described with reference to the drawings. Here, the Group 13 element nitride crystal substrate refers to a substrate made of a Group 13 element nitride crystal. The substrate is plate-shaped, that is, has a shape with a thickness that is relatively small compared to its width and depth (for example, 1 / 10 or less of the width or depth). The Group 13 element nitride crystal is, for example, Ga x Al y In 1-x-y N (where 0≦x≦1, 0≦y≦1), and specific examples include gallium nitride, aluminum nitride, indium nitride, or mixed crystals thereof. In this specification, the "main surface" of a Group 13 element nitride crystal means a surface present on the crystal that is separated in the thickness direction (the direction in which the crystal dimensions are smallest), and consists of two surfaces: a front surface (e.g., a device formation surface) and a back surface. In the following explanation, a method for producing a gallium nitride single crystal substrate will be described as a representative example, but other Group 13 element nitride crystal substrates can also be produced in a similar manner.

[0009] FIG. 1 is a flowchart showing an outline of a method for manufacturing a gallium nitride single crystal substrate according to an embodiment of the present disclosure.

[0010] <Preparation Step S1> As shown in Figure 1, in preparation step S1, first, a plate-shaped gallium nitride single crystal 7 (see, for example, Figure 6; hereinafter, sometimes abbreviated as single crystal 7) is prepared. For example, a slicing step is performed in which an ingot of gallium nitride single crystal produced by vapor phase growth is sliced ​​with, for example, a wire saw, to obtain a plate-shaped gallium nitride single crystal 7 whose main surface has a specific orientation. Before or after the slicing step, an outer shape processing step may be performed to process the outer shape of the single crystal 7 into a desired shape.

[0011] In the present disclosure, a gallium nitride single crystal 7 is used whose primary surface is a semipolar plane, a nonpolar plane, or an N-plane (nitrogen plane). Figures 2A to 2C respectively show the polar plane, semipolar plane, and nonpolar plane of a gallium nitride single crystal 7. In gallium nitride single crystal 7, single crystals whose primary surface is a polar plane (the c-plane or {0001} plane shown in Figure 2A) have established growth techniques and are commonly used planes. On the other hand, planes perpendicular to the polar plane, such as the m-plane ({1-100} plane) shown in Figure 2C, are nonpolar planes. Planes intermediate between polar and nonpolar planes, such as the {11-22} plane, {11-21} plane, {11-23} plane, {30-31} plane, {20-21} plane, {10-11} plane, and {10-12} plane shown in Figure 2B, are semipolar planes. Gallium nitride single crystal substrates with semipolar or nonpolar primary surfaces are expected to be applied to high-efficiency, high-output light-emitting devices. In Miller indices, ( ) represents a specific plane, {} represents an equivalent plane, [ ] represents a specific direction, and < > represents an equivalent direction. While negative numbers are typically represented by a bar above the number, this specification uses a minus sign (-) for convenience. For example, the {0001} plane includes the (0001) plane and the (000-1) plane. The {20-21} plane includes the (20-21) plane, the (20-2-1) plane, and their equivalent planes.

[0012] In the slicing step, for example, by slicing the c-plane grown gallium nitride single crystal obliquely to the c-plane (so that the main surface is inclined from both a polar and a nonpolar plane), a plate-shaped gallium nitride single crystal 7 having a semipolar main surface can be cut out. On the other hand, by slicing perpendicularly to the c-plane, a plate-shaped gallium nitride single crystal 7 having a nonpolar main surface can be cut out. In particular, it is preferable for the orientation of the main surface to be inclined 0° to 45° from the nonpolar plane toward the c-plane, since this results in a main surface with relatively little polarity. The polar c-plane refers to, for example, the (0001) plane and its opposite plane, the (000-1) plane. In Group 13 element nitride crystals, the c-plane is the Group 13 metal plane or the N-plane, which corresponds to the Ga-plane or N-plane in gallium nitride (GaN), respectively. By slicing the polar c-plane, a plate-shaped gallium nitride single crystal 7 having one main surface as the N-plane and the other as the Ga-plane can be cut out. The plate-shaped single crystal 7 cut out in the slicing step may be processed into a desired shape by dicing, laser processing, or the like. There are no particular limitations on the outer shape (planar shape) of the obtained single crystal 7, and it may be circular or polygonal. Furthermore, there are no particular limitations on the dimensions as long as it is plate-shaped (its thickness is relatively small compared to the dimensions of its main surface). This completes the preparation step S1.

[0013] <Backside Grinding Step S2> Next, the process moves to the backside grinding step S2 shown in FIG. 1. The backside grinding step S2 is primarily performed to process the single crystal 7 to the desired thickness and to flatten the backside and control the surface roughness. Specifically, the front surface of the single crystal 7 is attached to a base, and the backside is ground using, for example, lapping or grinding with a grinding wheel. Crystal defects and residual stresses caused by grinding may be removed by etching. The single crystal holder 2 used in the next step may be used as the base.

[0014] <Surface Grinding Step S3> Next, the process moves to the surface grinding step S3. The surface grinding step S3 is shown in Figures 3A and 3B. As the grinding device, a vertical-axis circular table type grinding device was used, as shown in Figures 3A and 3B, in which the rotation axis of the chuck table 3 on which the single crystal 7 is placed is parallel to the rotation axis of the grinding wheel holder 5 that holds the grinding wheel 4. First, as shown in Figure 3A, the gallium nitride single crystal 7 is attached and held together with the carrier 1 (see Figure 6) on the surface of the single crystal holder 2. For the single crystal holder 2, it is preferable to use a plate-like body with a larger area than the single crystal 7, and to hold multiple gallium nitride single crystals 7, for example, about three to a dozen, on the surface of the single crystal holder 2, in order to increase productivity.

[0015] The carrier 1 is a template that is attached to the single crystal holder 2 together with the gallium nitride single crystal 7. The carrier 1 in this embodiment is, for example, a plate-like body having the shape shown in FIG. 4 and is provided with multiple openings 11 for accommodating the gallium nitride single crystal 7. The openings 11 are recesses or through-holes. An embodiment using through-hole-type openings 11 will be described below. The carrier 1 shown in FIG. 3A is held on the surface of the single crystal holder 2 with the gallium nitride single crystal 7 accommodated in the multiple openings 11. The multiple openings 11 are arranged in a ring shape along the circumferential direction on the periphery of the carrier 1. This allows for a larger number of gallium nitride single crystals 7 to be processed simultaneously, thereby improving productivity. The openings 11 may also be arranged on multiple concentric circles. Furthermore, as shown in FIGS. 7B and 8B , within the plane of the single crystal 7, there is a tendency for the difference in grinding direction to increase in the width direction (circumferential direction) closer to the center of the carrier 1. If the opening 11 is located near the center of the carrier 1, it becomes difficult to control the grinding direction of the grinding wheel 4. Therefore, it is particularly preferable that the opening 11 be located radially away from the center of the carrier 1 at a distance of at least half the width of the opening 11 (i.e., one single crystal 7) (the circumferential dimension of the carrier 1, the long side direction of the rectangle in FIG. 6 ). Furthermore, since the grinding wheel track 8 has a curvature, the shorter the length of the opening 11 (the radial dimension of the carrier 1, the short side direction of the rectangle in FIG. 6 ) is relative to the diameter of the grinding wheel track 8, the easier it is to control the grinding direction of the grinding wheel 4 within the plane of the single crystal 7. For example, the width of the opening 11 may be less than half the diameter of the grinding wheel track 8. The carrier 1 is made of carbon fiber reinforced plastic (CFRP). CFRP has excellent strength, so as described below, a single carrier 1 can be used in both the grinding and CMP processes, avoiding the hassle of reattaching the carrier 1 and the loss of flatness that occurs when reattaching. CFRP uses carbon fiber as a reinforcing material and mainly uses thermosetting epoxy resin as a base material, but thermosetting resins such as unsaturated polyester resin and phenolic resin, as well as thermoplastic resins such as polyamide (PA), polycarbonate (PC), polyphenylene sulfide (PPS), and polyether ether ketone (PEEK) may also be used.By using such a CFRP carrier 1, it is possible to improve the productivity of gallium nitride single crystal substrates, reduce manufacturing costs, and further improve processing accuracy.

[0016] The single crystal holder 2 may be made of, for example, a silicon substrate, an alumina (Al 2 O 3 ) substrate, sapphire (single crystal alumina) substrate, silicon carbide (SiC) substrate, etc. can be used. To attach the carrier 1 containing the gallium nitride single crystal 7 to the single crystal holder 2, for example, an adhesive such as wax or an epoxy adhesive, or double-sided tape (adhesive tape with adhesive on both sides) may be used. The carrier 1 arranged around the gallium nitride single crystal 7 functions as a dummy that is ground together with the gallium nitride single crystal 7, improving the processing accuracy of the edge.

[0017] Next, as shown in Figure 3B, the single crystal holder 2 with the gallium nitride single crystal 7 attached is placed on the chuck table 3. The chuck table 3 has a porous surface and uses negative pressure to hold the single crystal holder 2 flat. The chuck table 3 can also be rotated around its central axis by a rotary drive source (not shown). It is also possible to hold the carrier 1 holding the gallium nitride single crystal 7 directly on the chuck table 3 without using the single crystal holder 2.

[0018] The grinding wheels 4 (see FIGS. 5A and 5B ) used to grind the gallium nitride single crystal 7 are, for example, rectangular and held by a wheel-shaped grinding wheel holder 5. The arrangement of the grinding wheels 4 on the grinding wheel holder 5 is not particularly limited; multiple elongated grinding wheels 4 may be arranged in a circular pattern at equal intervals around the circumferential direction of the grinding wheel holder 5, or may be arranged radially in the radial direction. Alternatively, disk-shaped or annular grinding wheels 4 may be used. In an embodiment in which multiple grinding wheels 4 are arranged in a circular pattern around the circumferential direction of the grinding wheel holder 5, the elongated grinding wheels 4 having a major axis and a minor axis are arranged with the major axis in the circumferential direction and the minor axis in the radial direction. In this case, the diameter of the orbits 8 and 8′ (see FIGS. 7A and 7B , 8A and 8B ) of the grinding wheels 4 (the pitch circle diameter of the grinding wheel 4) is greater than or equal to the width (diameter) of the region in which the single crystal 7 is disposed. The grinding wheels 4 may also be curved with a curvature corresponding to the orbits 8 and 8′. The grinding wheel 4 used may be, for example, a diamond grinding wheel or a SiC grinding wheel. The abrasive grains of the grinding wheel 4 are not particularly limited as long as they are capable of grinding the gallium nitride single crystal 7, but a grit size of #1000 to #5000 is preferred. After grinding with a grinding wheel 4 with a relatively large grit size and a low grit size (#1000 to #5000), grinding can be further performed with a grinding wheel 4 with a relatively small grit size and a high grit size (e.g., #6000 or higher). As shown in FIG. 3B , the grinding wheel holder 5 is fixed to the tip of the spindle 6, and the rotation of the spindle 6 rotates the grinding wheel holder 5 in the circumferential direction.

[0019] When grinding the gallium nitride single crystal 7, the single crystal holder 2 and the grindstone holder 5 are arranged opposite each other (see FIGS. 3B and 5A). The gallium nitride single crystal 7 and the grindstone 4 are pressed against each other with a predetermined pressure while rotating, grinding the main surface of the gallium nitride single crystal 7. The carrier 1 accommodates and holds the gallium nitride single crystal 7 in the peripheral opening 11 shown in FIG. 4. As shown in FIG. 5A, the positional relationship between the single crystal holder 2 and the grindstone holder 5 is adjusted so that the grindstone 4 passes near the center of the carrier 1. As shown in FIG. 5B, the chuck table 3 may be tilted with the center P as its apex. This allows the carrier 1 and the single crystal 7 to deform according to the shape of the chuck table 3, so that only a portion of the carrier 1 and the single crystal 7 comes into contact with the grindstone 4, thereby limiting the grinding area. This improves processability while reducing the load on the equipment and jigs, and also makes it easier to control the grinding direction, particularly for the single crystal 7 arranged near the center of the carrier 1. In FIG. 5B, the arrow L indicates the grinding region.

[0020] 3B and 5A, the single crystal holder 2 and the grindstone holder 5 rotate in the same direction, but they may also rotate in opposite directions. The rotation speed of the chuck table 3 holding the single crystal holder 2 is preferably 50 rpm or more and 500 rpm or less. The rotation speed of the grindstone 4 is greater than the rotation speed of the chuck table 3, and the rotation speed (circumferential speed) is preferably 10 m / sec or more and 50 m / sec or less. In addition, the feed speed of the grindstone 4 in the thickness direction of the single crystal 7 is preferably 0.01 μm / sec or more and 1.0 μm / sec or less.

[0021] In this embodiment, multiple openings 11 for accommodating the gallium nitride single crystal are provided along the circumferential edge of the carrier 1 (see FIG. 4 ). This increases productivity. In grinding, the wear on the carrier 1 can be reduced by allowing the main surface of the single crystal 7 to protrude beyond the main surface of the carrier 1. Furthermore, even when grinding the carrier 1 and the single crystal 7 together, if the material of the carrier 1 is harder (more difficult to grind) than the single crystal 7, the processing time or processing load must be increased. Therefore, it is preferable to use a carrier 1 with a hardness equal to or less than that of the single crystal 7 (with an equal or higher grinding rate) and to perform processing with the main surface of the single crystal 7 protruding beyond the main surface of the carrier 1 during processing. In this case, as shown schematically in FIG. 6 , the gap G between adjacent openings 11, 11 should be equal to or less than the track width W of the grinding wheel 4. During grinding, there is usually a difference in thickness between the carrier 1 and the single crystal 7 (the single crystal 7 is thicker). If the spacing between the openings 11, 11, i.e., the gap G between the main surfaces of the single crystals 7, 7 housed in these openings 11, 11, is larger than the track width W of the grinding wheel 4, when the single crystal 7 deviates from the grinding wheel track 8 due to rotation of the chuck table 3, the grinding wheel 4 may fall into the gap between the single crystals 7, causing the side of the grinding wheel 4 to collide with the corner of the single crystal 7, potentially chipping the grinding wheel 4 or the single crystal 7. If the grinding wheel 4 chips during grinding, the chipped pieces may become trapped, easily causing scratches on the single crystal 7. Here, the gap G refers to the shortest length separating the openings 11, 11. If the material of the carrier 1 is too soft (easily ground) compared to the single crystal 7, the carrier 1 will be significantly worn during grinding, resulting in reduced processing accuracy and increased manufacturing costs. Therefore, it is preferable that the hardness of the carrier 1 be equal to or slightly lower than that of the single crystal 7 (i.e., the grinding rate is equal to or slightly higher than that of the single crystal 7). The track width W of the grinding wheel 4 varies depending on the size of the device, but is preferably about 1 mm to 30 mm, for example.

[0022] When the rotation speed of the grinding wheel 4 is greater than the rotation speed of the chuck table 3, the trajectory 8 of the grinding wheel 4 passing through the main surface of the single crystal 7 during one rotation of the grinding wheel 4 is substantially arc-shaped. In the grinding process, it is preferable that the trajectory 8 of the grinding wheel 4 passes through the main surface of one single crystal 7 continuously only once during one rotation of the grinding wheel 4. In other words, it is preferable that the trajectory 8 of the grinding wheel 4 passing through the main surface of one single crystal 7 during the grinding process be a continuous arc that does not extend beyond the main surface of the single crystal 7. For example, in the example shown in FIG. 7A and FIG. 7B, which is an enlargement of portion A in the same figure, the grinding wheel trajectory 8 passes through each single crystal 7 only once. In contrast, in the example shown in FIG. 8A and FIG. 8B, which is an enlargement of portion A' in the same figure, the grinding wheel trajectory 8' passes through the main surface of one single crystal 7' in two separate segments (see portion C1 of the grinding wheel trajectory 8'). That is, twice, at portions b1 and b2 in FIG. 8B . If the single crystal 7' extends from the center to the outside in this way, the grinding wheel trajectory 8' passes over the main surface of the same single crystal 7' in two separate fragments, which tends to cause thickness variations within the surface due to the concentration of the surface pressure (processing load) of the grinding wheel 4. FIG. 9A is a schematic cross-sectional view of portion C1 showing the grinding wheel trajectory 8' including portions b1 and b2 in FIG. 8B , and FIG. 9B is a schematic cross-sectional view of portion C2 showing the grinding wheel trajectory 8' in FIG. 8B . As shown in FIG. 9A , when the area ratio occupied by the single crystal 7 in the grinding wheel 4 is low, the surface pressure applied to the single crystal 7 increases, resulting in a faster grinding speed. On the other hand, as shown in FIG. 9B , when the area ratio occupied by the single crystal 7 in the grinding wheel 4 is high, the surface pressure applied to the single crystal 7 decreases, resulting in a slower grinding speed. Therefore, if there are areas where the occupied area ratio is small and the surface pressure is high, such as parts b1 and b2 of the grinding wheel orbit 8', variations in thickness within the surface are likely to occur. In order to ensure that the orbit 8 of the grinding wheel 4 passes over the main surface of one single crystal 7 only once, it is advisable to adjust the dimensions of the single crystal 7 relative to the curvature of the orbit of the grinding wheel 4, particularly the radial dimension of the single crystal holder 2, and to do so it is advisable to shorten the radial length of the single crystal holder 2 of the single crystal 7.

[0023] In the grinding process of gallium nitride single crystals 7 whose main surfaces are nonpolar or semipolar, the processability and surface roughness vary depending on the incident direction (angle) of the grinding wheel 4. For example, as shown in Figure 10, a case will be described in which 18 semipolar single crystals 7 are attached to the surface of a single crystal holder 2. In Figure 10, the arrows indicate the direction of the

[0001] direction (the direction of the gallium face) of the single crystals 7 projected onto the main surface. The upper side (the direction of the arrow) of each single crystal 7 is the side closer to the gallium face, and the lower side is the side closer to the N face.

[0024] 11, the grinding direction of the grinding wheel 4 is represented by the angle formed between direction M, in which the [000-1] direction of the single crystal 7 is projected onto the main surface, and direction R1 in which the grinding wheel 4 grinds the main surface as the single crystal holder 2 and grinding wheel holder 5 rotate. In Fig. 11, the angle formed is 0° to 180° on the upstream side of the rotation direction R2 of the gallium nitride single crystal 7, and 0° to -180° on the downstream side.

[0025] Under these conditions, grinding was performed on the (20-2-1) plane (the main surface facing the [000-1] direction) of a semi-polar gallium nitride single crystal 7 whose main surfaces were the (20-21) plane and the (20-2-1) plane. It was found that the surface roughness of the gallium nitride single crystal 7 differed depending on the angle between the direction in which the grinding wheel 4 grinds the main surface of the gallium nitride single crystal 7 and the direction in which the c-axis of the gallium nitride single crystal 7 was projected onto the main surface (the surface roughness varied depending on the range of the angle). That is, when the surface roughness of each gallium nitride single crystal 7 after grinding was examined, it was found to be classified into angle ranges A to F shown in FIG. 12 and Table 1 below. Each range is represented by the angle between the direction in which the [000-1] direction of the gallium nitride single crystal 7 is projected onto the main surface and the direction in which the grinding wheel 4 grinds the main surface, with the upstream side of the rotation direction of the single crystal 7 being 0° to 180° and the downstream side being 0° to -180°. The grinding direction of the grinding wheel 4 was determined from the grinding marks (the trajectory of the grinding wheel 4) formed on the main surface. Table 1 shows the surface roughness for each angle range after grinding.

[0026] The specific processing conditions for obtaining the surface roughness (arithmetic mean height Sa) shown in Table 1 are: the rotation speed of the chuck table 3 is 100 rpm, the grinding wheel 4 is a #3000 diamond grinding wheel, the rotation speed (circumferential speed) of the grinding wheel 4 is 19 m / s, and the feed rate of the grinding wheel 4 is 0.12 μm / s or less. The arithmetic mean height Sa can be determined, for example, using a laser microscope VK-X1100 manufactured by Keyence Corporation. For example, the measurement mode is set to color ultra-depth, the measurement magnification is 1200x (50x objective, 24x eyepiece), the measurement range is approximately 60 μm x 80 μm, and the measurement pitch, cutoff filter λs, and cutoff filter λc are appropriately set according to the surface shape of the measurement area. The arithmetic mean height Sa is measured at multiple locations (5 or more points), and the average value is taken as the measured value. The thickness T of the single crystal 7 can also be determined using a micrometer.

[0027] As is clear from Table 1, in the ranges A, C, and E, the arithmetic mean height Sa of the gallium nitride single crystal 7 is larger than in the other ranges B, D, and F. That is, in the ranges B, D, and F, the main surface is close to a mirror finish, whereas in the ranges A, C, and E, the arithmetic mean height Sa is 0.2 μm or more, resulting in a so-called matte finish. It can also be seen that in the ranges A, C, and E, the thickness T of the gallium nitride single crystal 7 is smaller than in the other ranges B, D, and F (the amount of grinding is larger when compared with single crystals 7 having approximately the same initial thickness).

[0028] The surface ground by the #3000 grinding wheel 4 generally has a matte finish. Within ranges A, C, and E, the main surface of the single crystal 7 ground by the grinding wheel 4 has an arithmetic mean height (Sa) of 0.2 μm or more, suggesting that the grinding process was performed properly. On the other hand, within ranges B, D, and F, the main surface of the single crystal 7 ground by the grinding wheel 4 has an arithmetic mean height (Sa) of less than 0.2 μm, suggesting that the grinding process was not performed properly (despite the use of a grinding wheel, the grinding process was abrasive). In these ranges, it is expected that relatively large residual stresses are generated on the ground surface due to the grinding process not being performed properly. Furthermore, within ranges A, C, and E, the surface condition of the ground surface is relatively uniform. In the present disclosure, the grinding marks on the main surface of the single crystal 7 are formed by multiple arcs, and the grinding direction of the grinding wheel 4 varies within the main surface of the single crystal 7. In such a case, it is preferable that the grinding direction of the grinding wheel 4 (i.e., all grinding marks) be in the ranges A, C, and F over the entire area of ​​the main surface, but it is also good that the grinding direction of the grinding wheel 4 (i.e., more than half of the grinding marks) be in the ranges A, C, and F over at least half of the area of ​​the main surface.

[0029] In particular, the arithmetic mean height Sa is larger in range A than in other ranges. Furthermore, the surface condition of the processed surface in range A is particularly uniform compared to other ranges. Therefore, it is preferable to perform grinding so that the grinding direction of the grinding wheel 4 is within range A. After grinding is completed, the single crystal holder 2 is removed from the chuck table 3.

[0030] <CMP Step S4> Next, the process moves to CMP step S4. CMP step S4 is shown in FIG. 13. CMP is a process for polishing (mirror-finishing) the surface and eliminating minute distortions in the surface. FIG. 13 shows the configuration of a CMP processing apparatus. This apparatus includes a polishing pad 10 mounted on the surface of a rotating surface plate 9, and an alkaline slurry 12 containing abrasive grains is supplied onto the polishing pad 10. The carrier 1 and single crystal holder 2 containing the gallium nitride single crystal 7 are removed from the chuck table 3 of the grinding machine and then held on the underside of a support 13. In this state, the support 13 is rotated and pressed against the polishing pad 10. This causes a chemical reaction with the slurry 12, making the single crystal 7 more susceptible to polishing, and the single crystal 7 is then mechanically polished by the surface of the polishing pad 10. Examples of abrasive grains include silica, ceria, titania, zirconia, and alumina. The alkaline components of the slurry 12 other than the abrasive grains include, for example, an aqueous solution of sodium hydroxide, an aqueous solution of potassium hydroxide, etc. The pH of the slurry 12 is preferably adjusted to 8 or more and 14 or less.

[0031] 13, the rotation direction of the polishing pad 10 and the rotation direction of the support part 13 are the same, but they may be opposite directions. The slurry 12 may be dripped constantly or intermittently during the polishing process.

[0032] The carbon fiber reinforced plastic (CFRP) constituting the carrier 1 has high polishing resistance against the alkaline slurry 12, and therefore is hardly polished during the CMP process, resulting in little change in thickness. In contrast, if the carrier 1 contains silicon (Si), for example, glass fiber reinforced plastic (GFRP), and is subjected to CMP using the alkaline slurry 12, the difference in thickness from the single crystal 7 becomes large.

[0033] 14 is a graph showing the thickness difference between the carrier 1 and the single crystal 7 for various carrier materials after grinding in the surface grinding step (S3), in which the carrier 1 and the single crystal 7 were ground together, and after polishing in the CMP step (S4), in which the carrier 1 and the single crystal 7 were ground together using alkaline slurry 12. As a result, the thickness difference in the CMP step was particularly small, at 0.5 μm, for CFRP. CFRP also had small thickness variations after grinding and polishing.

[0034] Carrier 1 is GaN, Si, SiO 2 , GFRP, or CFRP, the thickness difference between the single crystal 7 and the carrier 1 after the co-grinding process can be 0 μm or more and 3 μm or less (the grinding rate is the same as or slightly higher than that of the single crystal 7). In particular, by forming the carrier 1 from CFRP, the thickness difference between the single crystal 7 and the carrier 1 after the CMP process (polishing) can be -1 μm or more and 1 μm or less (i.e., the polishing rates of the carrier 1 and the single crystal 7 are approximately the same). Using a carrier 1 made of a material whose thickness difference after co-grinding is greater than 1 μm (more easily polished than the single crystal 7) reduces processing accuracy and increases manufacturing costs due to a reduced number of times the carrier 1 can be used. Using a carrier 1 whose thickness difference after co-grinding is less than -1 μm (less easily polished than the single crystal 7) reduces processing accuracy and decreases the processing rate. Therefore, a carrier 1 made of a material whose thickness difference after co-grinding is -1 μm or more and 1 μm or less enables high-precision, low-cost processing. In particular, if the thickness difference after co-polishing is 0 μm or more, a relatively high polishing rate can be obtained. Note that the use of the carrier 1 in this embodiment is not limited to co-polishing. If the thickness of the single crystal 7 before polishing is made larger than that of the carrier 1 and the main surface of the single crystal 7 is processed so as to protrude from the main surface of the carrier 1, wear of the carrier 1 can be reduced, the number of times the carrier 1 can be used can be increased, and manufacturing costs can be reduced.

[0035] If the difference between the polishing rate of the carrier 1 and that of the single crystal 7 is large, a step will occur between the polished surface of the single crystal 7 and the carrier 1, resulting in a decrease in processing accuracy. A CFRP carrier 1 has a small difference in polishing rate with the single crystal 7 when using an alkaline slurry 12. This prevents the surface sagging of the single crystal 7 during polishing and improves flatness. Figure 15 is an explanatory diagram illustrating the surface sagging of the single crystal 7 during polishing in the CMP process. As shown in Figure 15A, the carrier 1 containing the single crystal 7 in the opening 11 is pressed against the polishing pad 10 by the support 13 and rotated while polishing. If the carrier 1 is made of a material that is easily polished, such as silicon, a thickness difference will occur between the carrier 1' and the single crystal 7, as shown in Figure 15B1. As a result, pressure will tend to concentrate on the edge 71 of the single crystal 7. Therefore, the single crystal substrate 141 obtained by polishing the single crystal 7 will have a large amount of polishing at the edge 71, resulting in so-called surface sagging and increased thickness variation, as shown in Figure 15C1. In contrast, when the carrier 1 is made of CFRP, there is almost no difference in thickness between the carrier 1 and the single crystal 7, so as shown in Fig. 15B2, the pressure is dispersed over the entire single crystal 7, and the single crystal substrate 14 obtained by polishing maintains flatness even at the edge 71, as shown in Fig. 15C2. In this way, when the carrier 1 is made of CFRP, the carrier 1 can be used repeatedly, which has the advantage of leading to reduced manufacturing costs.

[0036] As shown in FIG. 16A and FIG. 16B, which is an enlarged view of part M in FIG. 16B, the opening 11 provided in the carrier 1 is preferably at a distance d of 2 mm or more from the outer edge 15 of the carrier 1. By separating the opening 11 by 2 mm or more from the outer edge 15 of the carrier 1 in this manner, pressure is dispersed by the carrier 1 even at the end 71 close to the outer edge of the carrier 1, thereby suppressing sagging of the end 71. As a result, as shown in FIGS. 15B2 and 15C2, pressure is dispersed throughout the single crystal 7, and the polished single crystal substrate 14 can maintain flatness even at the end 71. Note that the carrier 1 typically has a disk shape with a diameter of 50 mm to 300 mm, but the carrier 1 is not limited to a disk shape and may be a polygonal shape such as a rectangle.

[0037] As described above in detail, according to this embodiment, the carrier 1 is made of CFRP, which has a grinding speed close to that of the substrate material (group 13 element nitride crystal) and is also resistant to the alkaline slurry used in CMP. This allows the same carrier 1 to be used from the grinding step to the CMP step. This improves productivity and processing accuracy, and reduces manufacturing costs.

[0038] Although the embodiments of the present disclosure have been described above, the present disclosure is not limited to the above-described embodiments, and various modifications and improvements are possible within the scope of the present disclosure.

[0039] REFERENCE SIGNS LIST 1, 1' Carrier 11 Opening 15 Outer edge 2 Single crystal holder 3 Chuck table 4 Grinding stone 5 Grinding stone holder 6 Spindle 7 Single crystal (nitride crystal of Group 13 element of the periodic table) 71 Edge 8 Grinding stone track 9 Surface plate 10 Polishing pad 11 Opening 12 Alkaline slurry 13 Support 14, 141 Single crystal substrate (nitride crystal substrate of Group 13 element of the periodic table)

Claims

1. a grinding step of storing a Group 13 element nitride crystal in a plurality of openings provided in a carrier and grinding a main surface of the crystal with a rotating grindstone while rotating the crystal; a chemical mechanical polishing step of chemically and mechanically polishing the ground main surface while the substrate is stored in the carrier; a chemical mechanical polishing step of polishing a substrate by a chemical mechanical polishing method using a slurry having an alkaline property, and a carrier made of a carbon fiber reinforced plastic.

2. 2. The method according to claim 1, wherein the periodic table group 13 element nitride crystal substrate is a gallium nitride single crystal substrate.

3. 3. The manufacturing method according to claim 1, wherein a plurality of the openings are provided along a circumferential direction of the peripheral edge of the carrier.

4. The method according to claim 3 , wherein a gap between the main faces of adjacent crystals housed in the opening is equal to or smaller than a track width of the grindstone.

5. 3. The manufacturing method according to claim 1, wherein in the grinding step, the orbit of the grinding wheel passes through the main surface of one of the crystals only once during one rotation of the grinding wheel.

6. The method according to claim 1 or 2, wherein the opening is spaced from an outer edge of the carrier by at least 2 mm.

7. 3. The method according to claim 1, wherein a thickness difference between the single crystal and the carrier after the grinding step (single crystal thickness-carrier thickness) is 0 μm or more.

8. 3. The method according to claim 1, wherein a thickness difference between the single crystal and the carrier after the grinding step (single crystal thickness-carrier thickness) is 0 μm or more and 3 μm or less.

9. 3. The method according to claim 1, wherein a difference in thickness between the single crystal and the carrier after the chemical mechanical polishing step is from −1 μm to 1 μm.