Method for producing molded object
Patent Information
- Application Number
- JP2024548115
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-07-31
- Filing Date
- 2023-07-31
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-07-31
AI Technical Summary
When integrally molding composite materials with reinforcing fibers and molding materials of higher fluidity, the composite material within the mold can shift, leading to misalignment and compromised physical properties, especially when using continuous fibers like plain weave cloth, where slight misalignment affects the desired properties and requires complex measures to prevent shifting.
A method involving fixing the composite material to a mold using multiple fixing members with a larger cavity area than the composite material, allowing the molding material with higher fluidity to flow without shifting the composite material, by using a pair of molds where the composite material is pressed and molded with the molding material, ensuring the composite material's position remains stable.
This method prevents the composite material from shifting during molding, maintaining its mechanical properties and improving shape followability, even with slight material flow, and allows for the production of complex shapes with ribs and bosses, while simplifying the molding process.
Abstract
Description
Manufacturing method of molded body
[0001] The present invention relates to a method for producing a molded article that is integrally molded from a composite material and an injection molding material that has higher fluidity than the composite material.
[0002] Composite materials using reinforcing fibers such as carbon fiber and glass fiber as reinforcements have high tensile strength and tensile modulus, and a small coefficient of linear expansion, resulting in excellent dimensional stability. Furthermore, they also have excellent heat resistance, chemical resistance, fatigue resistance, abrasion resistance, electromagnetic wave shielding properties, and X-ray transparency. For these reasons, composite materials are widely used in a variety of fields, including automobiles, sports and leisure, aerospace, and general industrial applications.
[0003]
[0003] Methods for manufacturing integrally molded articles from a plurality of different materials have been studied. For example, Patent Document 1 discloses a molding device in which pins are fitted into pin receiving holes while the peripheral edge of a skin material is pressed and clamped into the pin receiving holes, and the pins are pressed and held between the pressing surface of a skin material pressing frame and the skin material mounting surface of a lower mold. After molten thermoplastic resin is supplied between the skin material held in the lower mold and the molding surface of the upper mold, clamping begins. The molten thermoplastic resin flows, and the skin material is pressed by the clamping, stretched to conform to the mold shape and squeezed into the mold interior. At the same time, the peripheral edge of the skin material slides between the pins and the pin receiving holes and between the pressing surface and the skin material mounting surface, and is drawn toward the interior of the mold.
[0004] Patent Document 2 discloses the use of a mold for producing a fiber-reinforced thermoplastic resin molded product by press-molding a sheet material in which a discontinuous fiber-reinforced thermoplastic resin layer is laminated on at least a portion of one side of a continuous fiber-reinforced thermoplastic resin layer, in which a frame-shaped dam portion is provided on the outer periphery of the cavity when the upper and lower molds are closed, to prevent the discontinuous fiber-reinforced thermoplastic resin layer from flowing out of the cavity, while forming a gap that allows the continuous fiber-reinforced thermoplastic resin layer to extend out of the cavity.
[0005] Patent Document 3 discloses that an auxiliary mold that is in close contact with the outer peripheral wall of the lower mold of a stamping mold and can slide up and down is arranged, and when a molten thermoplastic resin between the upper and lower molds of the stamping mold is press-molded to form a substrate and a skin material is pressure-bonded to the substrate, the auxiliary mold prevents the molten material from leaking from between the upper and lower molds.
[0006] Patent Document 4 describes a method for producing an injection-molded product containing multiple sheets at lower cost. In Patent Document 4, multiple resin-impregnated reinforcing member sheets with holes are arranged, a movable mold is moved to clamp the mold, and resin is injected to fill the spaces between the resin-impregnated reinforcing member sheets.
[0007] Japanese Patent No. 3413356 Japanese Patent No. 5855401 Japanese Patent Publication No. 9-117922 Japanese Patent Publication No. 2020-179549
[0008] However, when multiple materials with different fluidities are molded together in a mold, there is a problem that the material with higher fluidity flows within the mold, causing the material with lower fluidity to shift position within the mold.
[0009] In the method of Patent Document 1, the skin material is fixed by holding it on the outer periphery of the mold, but the method of Patent Document 1 cannot be applied to molding in which a material with low fluidity is placed completely within the cavity of the mold, such as insert molding.
[0010] In the method of Patent Document 2, a dam portion is provided at the outer peripheral edge of the cavity to prevent the discontinuous fiber reinforced thermoplastic resin layer from flowing out, but no method for fixing the sheet material is described.
[0011] In the method of Patent Document 3, the skin material is held outside the mold by a jig, but the method of Patent Document 3 cannot be applied to molding in which a material with low fluidity is placed completely inside the mold cavity, such as insert molding.
[0012] The method of Patent Document 4 uses a reinforcing member resin-impregnated sheet made of a plain-woven cloth made of glass fibers with a wire diameter of approximately 17 μm, impregnated with polypropylene resin. When using a material in which the reinforcing fibers are continuous and oriented in a specific direction, such as a plain-woven cloth, even slight misalignment (even a few millimeters) during press molding after injection molding makes it difficult to obtain the desired physical properties. Therefore, measures such as modifying the molding die to prevent misalignment of the reinforcing member resin-impregnated sheet are necessary. In particular, when attempting to impregnate resin between multiple reinforcing members, the process becomes too complicated.
[0013] An object of the present invention is to provide a method for manufacturing a molded body that can prevent the composite material from shifting position within a mold when integrally molding a composite material and a molding material that has higher fluidity than the composite material, without fixing the composite material on the outer periphery of the cavity of the mold.
[0014] In order to solve the above problems, the present invention provides the following means. <1> A method for producing a molded body integrally molded from a composite material containing reinforcing fibers dispersed in an in-plane direction and a molding material having a higher fluidity than the composite material, the method comprising the following steps (1) to (3): (1) fixing the composite material to a first molding die using a plurality of fixing members provided on the first molding die, the first molding die having a cavity with an area larger than that of the composite material in a plan view; (2) moving a second molding die toward the composite material fixed to the first molding die and bringing the second molding die into contact with the composite material; and (3) pressing the composite material and the molding material together using the first molding die and the second molding die to integrally mold them. <2> The method for producing a molded body according to <1>, further comprising a step of releasing the fixing of the composite material by the fixing members. <3> The method for producing a molded body according to <1> or <2>, further comprising a step of laminating the molding material onto the composite material before step (1). <4> The method for producing a molded body according to <3>, wherein in step (1), the composite material is fixed to the first molding die so that the molding material contacts the first molding die. <5> The method for producing a molded body according to <1> or <2>, wherein in step (1), the composite material is fixed to the first molding die so that the molding material is positioned on the opposite side of the first molding die. <6> The method for producing a molded body according to <1> or <2>, comprising, after step (1) and before step (2), a step of laminating the molding material onto the composite material. <7> The method for producing a molded body according to <1> or <2>, wherein the molding material is an injection molding material, and comprises, after step (2) and before step (3), a step of injecting the molding material between the first molding die and the second molding die. <8> The method for producing a molded body according to <2>, wherein the molding material is an injection molding material, and the method includes, after the step (2) and before the step of releasing the fixing of the composite material by the fixing member, a step of injecting the molding material between the first molding die and the second molding die. <9> The method for producing a molded body according to <7> or <8>, wherein the molding material is injected between the first molding die and the composite material.<10> The method for producing a molded body according to <7> or <8>, wherein the molding material is injected between the second mold and the composite material. <11> The method for producing a molded body according to any one of <1> to <10>, wherein the first mold and the second mold are a pair of female and male molds. <12> The method for producing a molded body according to <11>, wherein the first mold is a fixed mold and the second mold is a movable mold. <13> The method for producing a molded body according to <11> or <12>, wherein the first mold is a lower mold and the second mold is an upper mold. <14> The method for producing a molded body according to any one of <1> to <13>, wherein the fixing member is a hole forming member that forms holes in the molded body. <15> The method for producing a molded body according to any one of <1> to <14>, wherein the reinforcing fibers are randomly dispersed in two-dimensional directions in the in-plane direction of the composite material. <16> The method for manufacturing a molded body according to <12>, wherein the molding material is an injection molding material, and includes a step of injecting the injection molding material between the first molding die and the second molding die after step (2) and before step (3), wherein the injection is carried out from the first molding die. <17> The method for manufacturing a molded body according to <16>, wherein a design surface is formed by the second molding die, and the injection molding material is filled between the second molding die and the composite material. <18> The method for manufacturing a molded body according to <17>, wherein one or more flow holes are formed in the composite material to allow the injection molding material to pass through, and the injection molding material injected from the first molding die is injected between the first molding die and the second molding die by flowing through the flow holes. <19> The method for manufacturing a molded body according to <18>, wherein the first molding die has a first gate, which is a gate for injecting an injection molding material into the molding die, in a region where the composite material is placed in a plan view. <20> The method for manufacturing a molded body according to <16>, wherein a design surface is formed by the second molding die, and a resin sheet is placed between the second molding die and the composite material.<21> The method for manufacturing a molded body according to <17> or <20>, wherein the design surface has a grain pattern formed by the second molding die. <22> The method for manufacturing a molded body according to any one of <1> to <12>, wherein the first molding die is a fixed die and the second molding die is a movable die, and the method for manufacturing a molded body by opening and closing the second molding die by moving it horizontally, wherein there are at least two or more fixing members positioned differently in the height direction. <23> The method for manufacturing a molded body according to any one of <1> to <12>, wherein the first molding die is a fixed die and the second molding die is a movable die, and the method for manufacturing a molded body by opening and closing the second molding die by moving it horizontally, wherein there are at least two or more fixing members positioned differently in the horizontal direction. <24> The method for manufacturing a molded body according to any one of <1> to <23>, wherein the composite material has a shape obtained by pattern cutting. <25> The method for manufacturing a molded body according to <19>, wherein the first molding die has second gates for injecting the injection molding material into an area other than the area where the composite material is placed in a plan view, and the number n1 of the first gates and the number n2 of the second gates satisfy 0 < n1 < n2. <26> The method for manufacturing a molded body according to <19> or <25>, wherein the first molding die has second gates for injecting the injection molding material into an area other than the area where the composite material is placed in a plan view, and the discharge rate V1 of the injection molding material from the first gate and the discharge rate V2 of the injection molding material from the second gate satisfy 0 < V1 < V2.
[0015] According to the method for producing a molded article of the present invention, when a composite material and a molding material having higher fluidity than the composite material are integrally molded, the composite material does not need to be fixed on the outer periphery of the cavity of the mold, and displacement of the composite material within the mold can be prevented. By using a composite material containing reinforcing fibers dispersed in the in-plane direction, even if the composite material flows slightly during molding, its basic mechanical properties do not change significantly. Furthermore, shape conformability is improved compared to those using continuous fibers such as plain weave cloth.
[0016] FIG. 1 is a cross-sectional view of a molded body 1 according to a first embodiment of the present invention. FIG. 2 is a schematic diagram showing a method for manufacturing the molded body 1 according to the first embodiment. FIG. 3 is a schematic diagram showing a method for manufacturing the molded body 1 according to the first embodiment. FIG. 4 is a schematic diagram showing a method for manufacturing the molded body 1 according to the first embodiment. FIG. 5 is a schematic diagram showing a method for manufacturing the molded body 1 according to the first embodiment. FIG. 6 is a cross-sectional view of a molded body 101 according to a second embodiment of the present invention. FIG. 7 is a schematic diagram showing a method for manufacturing the molded body 101 according to the second embodiment. FIG. 8 is a schematic diagram showing a method for manufacturing the molded body 101 according to the second embodiment. FIG. 9 is a schematic diagram showing a method for manufacturing the molded body 101 according to the second embodiment. FIG. 10 is a schematic diagram showing a method for manufacturing the molded body 101 according to the second embodiment. FIG. 11 is a schematic diagram showing a method for manufacturing the molded body 101 according to the second embodiment. FIG. 12 is a schematic diagram showing a method for manufacturing the molded body 201 according to the third embodiment. FIG. 13 is a schematic diagram showing a method for manufacturing the molded body 201 according to the third embodiment. FIG. 14 is a schematic diagram showing a method for manufacturing the molded body 201 according to the third embodiment. FIG. 15 is a schematic diagram showing a method for manufacturing the molded body 201 according to the third embodiment. 1 is a schematic diagram showing a method for manufacturing a molded body 201 of a third embodiment; FIG. 2 is a schematic diagram showing a method for manufacturing a molded body 201 of a third embodiment; FIG. 3 is a schematic diagram showing a method for manufacturing a molded body 301 of a fourth embodiment; FIG. 4 is a schematic diagram showing a method for manufacturing a molded body 301 of a fourth embodiment; FIG. 5 is a schematic diagram showing a method for manufacturing a molded body 301 of a fourth embodiment; FIG. 6 is a schematic diagram showing a method for manufacturing a molded body 301 of a fourth embodiment; FIG. 7 is a schematic diagram showing a method for manufacturing a molded body 301 of a fourth embodiment; FIG. 8 is a schematic diagram showing a method for manufacturing a molded body 301 of a fourth embodiment; FIG. 9 is a horizontal cross-sectional view showing a first molding die 410 and a second molding die 420 that are provided so as to be able to open and close in the horizontal direction; FIG. 10 is a perspective view showing a box-shaped molded body 100; FIG. 11 is a schematic diagram of a composite material having a pattern-cut shape; FIG. 12 is a front view showing the first molding die in a state in which the pattern-cut composite material is fixed by fixing members; FIG. 13 is a horizontal cross-sectional view showing a first molding die 510 and a second molding die 520 to which a composite material is fixed by fixing members 512; FIG. 14 is a plan view of a first molding die 610.
[0017]
[0023] Hereinafter, embodiments of the present invention will be described in detail. [First Embodiment] Fig. 1 is a schematic cross-sectional view of a molded body 1 according to a first embodiment of the present invention, and Figs. 2 to 6 are schematic views showing a method for manufacturing the molded body 1. The molded body 1 is integrally molded with a reinforcing portion 2 formed from a composite material 2A and a main body portion 3 formed from a molding material 3B that has higher fluidity than the composite material 2A.
[0018] [Composite Material] The composite material 2A includes reinforcing fibers and a matrix resin. In the composite material 2A, the reinforcing fibers are dispersed in the in-plane direction within the matrix resin.
[0019] [Reinforcing Fiber] The reinforcing fiber is preferably at least one selected from the group consisting of carbon fiber, aramid fiber, and glass fiber, and more preferably carbon fiber or glass fiber.
[0020] [Carbon Fiber] 1. Carbon Fibers in General Generally known carbon fibers include polyacrylonitrile (PAN)-based carbon fibers, petroleum / coal pitch-based carbon fibers, rayon-based carbon fibers, cellulose-based carbon fibers, lignin-based carbon fibers, and phenol-based carbon fibers. Any of these carbon fibers can be suitably used in the present invention. Of these, polyacrylonitrile (PAN)-based carbon fibers are preferred in the present invention because of their excellent tensile strength. As a PAN-based carbon fiber, for example, TENAX (registered trademark) STS40-24KS carbon fiber (average fiber diameter 7 μm) manufactured by Teijin Limited can be used.
[0021] 2. Sizing Agent for Carbon Fiber The carbon fiber may have a sizing agent attached to its surface. When using carbon fiber with a sizing agent attached, the type of sizing agent can be appropriately selected depending on the type of carbon fiber and the type of resin used in the composite material or injection molding material, and is not particularly limited.
[0022] [Glass Fiber] 1. Glass Fiber in General The glass fiber may be any glass fiber that is generally called glass fiber. The glass composition of glass fiber such as A glass, C glass, E glass, etc. specified in JIS R3140:2006 is not particularly limited, and TiO may be used in some cases. 2 , S.O. 3 , P 2 O 5 The glass fiber may contain components such as E-glass RS240QR-483 (count: 2400 g / 1000 m) manufactured by Nitto Boseki Co., Ltd., for example.
[0023] 2. Sizing Agent for Glass Fiber The glass fiber may have a sizing agent attached to its surface. When using glass fiber with a sizing agent attached, the type of sizing agent can be appropriately selected depending on the type of glass fiber and the type of resin, and is not particularly limited. Glass fiber that has been pre-treated with a conventionally known coupling agent such as an organosilane compound, an organotitanium compound, an organoborane compound, or an epoxy compound can be preferably used.
[0024] [Dispersion in the in-plane direction] The reinforcing fibers contained in the composite material are preferably dispersed in the in-plane direction. Dispersion of the reinforcing fibers in the in-plane direction means that the fiber axes of the reinforcing fibers are dispersed so as to face the in-plane direction. It is preferable that the angle between the fiber axes of the reinforcing fibers and the in-plane direction is 45° or less.
[0025] 1. In-plane direction The composite material 2A is preferably a plate-shaped material. The in-plane direction is any direction parallel to a plane perpendicular to the plate thickness direction of the composite material 2A.
[0026] 2. Randomly Dispersed in Two Dimensions The reinforcing fibers are preferably randomly dispersed in two dimensions in the in-plane direction of the composite material 2A. When the composite material 2A is press-molded without flow, the shape of the reinforcing fibers is largely maintained before and after molding. Therefore, it is preferable that the reinforcing fibers contained in the reinforcing portion 2 formed from the composite material 2A are similarly randomly dispersed in two dimensions in the in-plane direction. Here, "randomly dispersed in two dimensions" refers to a state in which the reinforcing fibers are oriented randomly in the in-plane direction of the composite material 2A or the reinforcing portion 2, rather than in a specific direction such as one direction, and are arranged in the sheet plane overall without showing a specific directionality. The composite material 2A (or the reinforcing portion 2) obtained using discontinuous fibers randomly dispersed in this way is substantially isotropic, not anisotropic in-plane.
[0027] The degree of orientation, which represents the degree to which the reinforcing fibers are randomly dispersed in two dimensions in the in-plane direction of the composite material 2A or the reinforcing portion 2, is evaluated by calculating the ratio of the tensile modulus of the composite material 2A in two mutually perpendicular directions. The reinforcing fibers can be evaluated as being randomly dispersed in two dimensions if the (Eδ) ratio, calculated by dividing the larger of the tensile modulus values measured in any direction of the composite material 2A (or the reinforcing portion 2) by the smaller of the measured values, is 5 or less, more preferably 2 or less, and even more preferably 1.5 or less. When the reinforcing portion 2 has a curved surface, the degree of two-dimensional random dispersion (orientation) of the reinforcing fibers in the in-plane direction of the reinforcing portion 2 can be evaluated by heating the molded body 1 to a softening temperature or higher to return it to a flat plate shape, removing only the reinforcing portion 2, and then solidifying it. Then, a test piece is cut out from the reinforcing portion 2 that has been returned to a flat plate shape, and the tensile modulus of the test piece in two mutually perpendicular directions is measured, thereby evaluating the two-dimensional random dispersion in the reinforcing portion 2.
[0028] [Fiber length of reinforcing fibers contained in composite material] The weight-average fiber length LwA of the reinforcing fibers contained in composite material 2A is preferably 1 mm or more, more preferably 3 mm or more. If LwA is 100 mm or less, the fluidity of the material is less likely to decrease when press-molding composite material 2A to produce it, and the reinforcing portion 2 can be easily formed into a desired shape. Furthermore, if LwA is 1 mm or more, the mechanical strength of the resulting reinforcing portion 2 is less likely to decrease, which is preferable.
[0029] Since the weight average fiber length LwA of the reinforcing fibers contained in composite material 2A does not change before and after molding, the weight average fiber length LwA of the reinforcing fibers contained in composite material 2A can be determined by examining the weight average fiber length of the reinforcing fibers contained in reinforcing portion 2. The weight average fiber length LwA of the reinforcing fibers contained in composite material 2A is preferably 3 mm or more and 100 mm or less, more preferably 3 mm or more and 80 mm or less, and even more preferably 5 mm or more and 60 mm or less. The weight average fiber length of the reinforcing fibers can be calculated using equation (1) described below.
[0030] [Molding Material] The molding material 3B forming the main body 3 contains a matrix resin. Furthermore, the molding material 3B preferably contains reinforcing fibers. The reinforcing fibers contained in the molding material 3B are preferably the carbon fibers or glass fibers described above. The molding material 3B has higher fluidity than the composite material 2A. A molding material 3B having higher fluidity than the composite material 2A can be produced by lowering the fiber volume fraction (Vf) of the molding material 3B compared to the fiber volume fraction (Vf) of the composite material 2A. Furthermore, by shortening the weight-average fiber length of the reinforcing fibers contained in the molding material 3B compared to the weight-average fiber length of the reinforcing fibers contained in the composite material 2A, the fluidity of the molding material 3B can be increased compared to the fluidity of the composite material 2A.
[0031] [Fiber length of reinforcing fibers contained in molding material] Molding material 3B contains reinforcing fibers with a weight-average fiber length LwB, and it is preferable that LwB < LwA. When LwB < LwA, the mechanical strength of reinforcing portion 2 formed from composite material 2A is higher than the mechanical strength of main body portion 3 formed from molding material 3B, and therefore reinforcing portion 2 can reinforce molded body 1.
[0032] The molding material 3B may be an injection molding material. When the molding material 3B is injected into a mold to form the main body 3, the molding material 3B immediately before injection is called the injection molding material. When the molding material 3B is mixed before injection, the mixed molding material 3B is called the injection molding material.
[0033] The weight-average fiber length LwB of the reinforcing fibers contained in the molding material 3B is preferably less than 3 mm. The weight-average fiber length LwB is more preferably 0.01 mm or more and less than 3 mm. The lower limit of the weight-average fiber length LwB is preferably 0.01 mm or more, more preferably 0.05 mm or more, and even more preferably 0.1 mm or more. When the weight-average fiber length LwB is 0.01 mm or more, the mechanical strength of the main body portion 3 is ensured. On the other hand, the upper limit of the weight-average fiber length LwB is preferably less than 3 mm, more preferably less than 2 mm, and even more preferably less than 1 mm.
[0034] When the weight-average fiber length LwB is 1.0 mm or less, the main body 3 can be manufactured using an injection molding material kneaded with the molding material 3B. Generally, the weight-average fiber length LwB of the reinforcing fibers contained in the injection molding material sufficiently kneaded with the molding material 3B is less than 1 mm. The weight-average fiber length of the reinforcing fibers can be calculated using the formula (1) described below.
[0035] [Weight average fiber length Lw] Generally, the fiber length of each reinforcing fiber is L i Then, the weight average fiber length Lw can be calculated by the following formula (1): The unit of the weight average fiber length Lw is mm.
[0036] Here, "I" indicates the number of measured reinforcing fibers. The reinforcing fibers can be extracted from the reinforcing portion 2 and the main body portion 3 by, for example, performing a heat treatment at 500°C for about 1 hour and removing the matrix resin in a furnace. The weight-average fiber length Lw is, for example, the fiber length L of 100 fibers (I=100) randomly extracted from the reinforcing portion 2 and the main body portion 3 after the heat treatment. 1 ~L 100 can be measured to the nearest 1 mm using a caliper or the like and calculated based on formula (1).
[0037] When short reinforcing fibers that cannot be measured with a caliper are included, the matrix resin is removed, and the resulting reinforcing fibers are put into water containing a surfactant, and the mixture is thoroughly stirred with ultrasonic vibrations. The stirred dispersion of reinforcing fibers is randomly sampled with a measuring spoon to obtain an evaluation sample, and the length of 3,000 reinforcing fibers (I=3,000) is measured using an image analyzer Luzex AP manufactured by Nireco Corporation. 1 ~L 3000 The weight average fiber length Lw can be calculated in the same manner as in the above formula (1) using the above formula.
[0038] [Volume fraction of reinforcing fibers in composite material and molding material] The volume fraction of reinforcing fibers (Vf) can be calculated for each of composite material 2A and molding material 3B using the following formula (2). There are no particular limitations on the volume fraction of reinforcing fibers, but the volume fraction of reinforcing fibers (Vf) is preferably 10 to 60 Vol%, more preferably 20 to 50 Vol%, and even more preferably 25 to 45 Vol%. Volume fraction of reinforcing fibers (Vf) = 100 × volume of reinforcing fibers / (volume of reinforcing fibers + volume of resin) Formula (2) In the present invention, it is preferable from the perspective of the manufacturing process that the volume fraction of reinforcing fibers (Vfb) of molding material 3B and the volume fraction of carbon fibers (Vfa) of composite material 2A satisfy the relationship Vfa ≧ Vfb. For example, when crushed scraps of composite material 2A recovered from the manufacturing process or product are used as molding material 3B, or when crushed scraps are further added with a thermoplastic resin and used as molding material 3B to manufacture main body 3, Vfa > Vfb is often the case. In other words, adopting a manufacturing method that satisfies Vfa ≥ Vfb allows for efficient use of scraps remaining after cutting out composite material 2A and facilitates material recycling. Vfa is preferably 20 to 45 Vol%, more preferably 25 to 40 Vol%. Vfb is preferably 1 to 40 Vol%, more preferably 5 to 30 Vol%, and even more preferably 10 to 25 Vol%.
[0039] [Analysis of Reinforcing Fiber Volume Fraction (Vf)] Although there are no limitations on the analysis of the reinforcing fiber volume fraction, it is recommended to measure it as follows. A sample is cut out from the reinforcing portion 2 or the main body portion 3, and the resin is burned off in a furnace at 500°C for 1 hour. The masses of the reinforcing fibers and resin are calculated by weighing the mass of the sample before and after treatment. Next, the volume fraction of the reinforcing fibers and resin is calculated using the specific gravity of each component. Vf = 100 x reinforcing fiber volume / (reinforcing fiber volume + resin volume)
[0040] [Resin] The matrix resin contained in the composite material 2A and the matrix resin contained in the molding material 3B may be either thermosetting or thermoplastic.
[0041] 1. Thermoplastic Resin 1.1 Overview When the resin used is a thermoplastic resin, the type is not particularly limited, and a resin having a desired softening point or melting point can be appropriately selected and used. As the thermoplastic resin, one having a softening point in the range of 180°C to 350°C is usually used, but is not limited thereto.
[0042] Examples of thermoplastic resins include polyolefin resins, polystyrene resins, polyamide resins, polyester resins, polyacetal resins (polyoxymethylene resins), polycarbonate resins, (meth)acrylic resins, polyarylate resins, polyphenylene ether resins, polyimide resins, polyethernitrile resins, phenoxy resins, polyphenylene sulfide resins, polysulfone resins, polyketone resins, polyether ketone resins, thermoplastic urethane resins, fluorine-based resins, and thermoplastic polybenzimidazole resins.
[0043] The thermoplastic resin used in the composite material 2A and the molding material 3B may be one type or two or more types. Examples of the use of two or more types of thermoplastic resins in combination include, but are not limited to, the use of thermoplastic resins with different softening points or melting points, or the use of thermoplastic resins with different average molecular weights. When a thermoplastic resin is used, it is more preferable to use a polyolefin resin, and even more preferable to use a polypropylene resin.
[0044] 1.2 Resins of the Composite Material and Molding Material The resin contained in composite material 2A is preferably a thermoplastic resin. If the resin contained in composite material 2A is a thermoplastic resin, it is more preferable that the resins contained in composite material 2A and molding material 3B are the same type of thermoplastic resin.
[0045] 2. Thermosetting Resin The resin contained in the composite material 2A may be a thermosetting resin. In this case, a sheet molding compound using reinforcing fibers may be used as the composite material 2A. Due to its high moldability, the sheet molding compound can be easily molded into even complex shapes. The sheet molding compound has higher fluidity and shapeability than continuous fibers, making it easy to create ribs and bosses.
[0046] [Other Agents] The resin used in the composite material 2A and the molding material 3B may contain additives such as various fibrous or non-fibrous fillers such as organic or inorganic fibers, flame retardants, UV-resistant agents, stabilizers, release agents, pigments, softeners, plasticizers, surfactants, etc., within the scope of the present invention.
[0047] [Preferred Combinations of Resins and Fibers] [Fibers] The reinforcing fibers contained in the composite material 2A are preferably glass fibers and / or carbon fibers, and the reinforcing fibers contained in the molding material 3B are preferably glass fibers. Carbon fibers may be used partially as the reinforcing fibers contained in the composite material 2A, and glass fibers may be used in the portions other than the portions using carbon fibers. The portions in which carbon fibers are used in the composite material 2A are preferably the portions surrounding holes 2H (described later) in the reinforcing portion 2.
[0048] [Resin] The resin contained in composite material 2A may be a thermoplastic resin or a thermosetting resin, and the resin contained in molding material 3B may be a thermoplastic resin or a thermosetting resin. While molding material 3B contains a thermoplastic resin, a thermosetting sheet molding compound may be used for composite material 2A.
[0049] It is preferable that the volume Va of the composite material 2A used in the reinforcing portion 2 and the volume Vb of the molding material 3B used in the main body portion 3 satisfy the relationship Vb≧Va. Va:Vb is preferably 10:90 to 50:50, and more preferably 20:80 to 40:60.
[0050] [Manufacturing Method] Next, a description will be given of a method for manufacturing the molded body 1. In this embodiment, the molded body 1 is integrally molded from a composite material 2A containing reinforcing fibers dispersed in the in-plane direction and a molding material 3B having higher fluidity than the composite material 2A.
[0051] The manufacturing method for producing the molded body 1 includes the following steps (1) to (3): (1) a step of fixing the composite material 2A to the first molding die 10 using a plurality of fixing members 12 provided on the first molding die 10, which has a cavity 11 with an area larger than that of the composite material 2A in a planar view; (2) a step of moving the second molding die 20 toward the composite material 2A fixed to the first molding die 10 and bringing the second molding die 20 into contact with the composite material 2A; (3) a step of pressing the composite material 2A and the molding material 3B together using the first molding die 10 and the second molding die 20 to mold them into a single unit.
[0052] The molding material 3B may be introduced into the mold at any timing prior to step (3). For example, a step of laminating the molding material 3B on the composite material 2A may be included prior to step (1). That is, in step (1), it is preferable to fix the laminate of the composite material 2A and the molding material 3B in a stacked state in the cavity 11 of the first molding die 10 using a plurality of fixing members 12. In this case, it is preferable to fix the composite material 2A to the first molding die 10 in step (1) so that the molding material 3B contacts the first molding die 10.
[0053] When the resin contained in the composite material 2A and the molding material 3B is a thermoplastic resin, it is preferable to use cold press molding.
[0054] The manufacturing method for producing a molded body 1 by cold press molding includes the following steps (0) to (3): (0) a step of heating a composite material 2A and a molding material 3B to a first predetermined temperature; (1) a step of fixing the composite material 2A and the molding material 3B to a first molding die 10 using a plurality of fixing members 12 provided on the first molding die 10, which has a cavity 11 with an area larger than that of the composite material 2A in a planar view; (2) a step of moving a second molding die 20 toward the composite material 2A fixed to the first molding die 10 and bringing the second molding die 20 into contact with the composite material 2A; (3) a step of pressing the composite material 2A and the molding material 3B together using the first molding die 10 and the second molding die 20 to mold them into a single unit.
[0055] (0) Step of heating composite material 2A to a first predetermined temperature It is preferable to heat composite material 2A to a first predetermined temperature in advance. When the thermoplastic resin contained in composite material 2A is crystalline, the first predetermined temperature is a temperature equal to or higher than the melting point and equal to or lower than the decomposition temperature of the thermoplastic resin. When the thermoplastic resin contained in composite material 2A is amorphous, the first predetermined temperature is a temperature equal to or higher than the glass transition temperature and equal to or lower than the decomposition temperature of the thermoplastic resin.
[0056] In the case of cold press molding, the temperatures of the first molding die 10 and the second molding die 20 are adjusted to a second predetermined temperature. If the thermoplastic resin contained in the composite material 2A is crystalline, the second predetermined temperature is a temperature below the melting point of the thermoplastic resin. If the thermoplastic resin contained in the composite material 2A is amorphous, the second predetermined temperature is a temperature below the glass transition temperature of the thermoplastic resin. By adjusting the temperatures of the composite material 2A and the first molding die 10 in this way, cold pressing can be performed suitably.
[0057] First, as shown in Figure 2, a composite material 2A is fixed in a cavity 11 of a first molding die 10 by a plurality of fixing members 12. The fixing members 12 may be, for example, slide cores that form holes 1H in the molded body 1. For example, holes 2H may be formed in the composite material 2A beforehand, and the fixing members 12 may be inserted into the holes 2H to fix the composite material 2A. Alternatively, the composite material 2A may be fixed by piercing pin-shaped fixing members 12 into the composite material 2A. In this case, holes 2H need not be formed in the composite material 2A.
[0058] The composite material 2A may be pre-shaped and then placed in the cavity 11 of the first molding die 10 so as to fit the cavity 11 of the first molding die 10 .
[0059] Next, as shown in FIG. 3, the second molding die 20 is moved toward the composite material 2A fixed to the first molding die 10, and the second molding die 20 is brought into contact with the composite material 2A.
[0060] Next, as shown in Figure 4, the composite material 2A and molding material 3B are pressed together using a first molding die 10 and a second molding die 20 to form an integral mold. The molding pressure is not particularly limited, but is preferably less than 20 MPa, and more preferably 10 MPa or less. When the composite material 2A and molding material 3B are pressed together in this manner, molding material 3B, which has higher fluidity than composite material 2A, flows within the mold. Even in this case, composite material 2A is fixed by fixing member 12, so that displacement of the composite material 2A can be prevented.
[0061] When composite material 2A and molding material 3B are pressed together, hole 2H is formed in composite material 2A at a position corresponding to fixing member 12, and hole 3H is formed in molding material 3B at a position corresponding to fixing member 12. In other words, fixing member 12 is a hole-forming member that forms hole 1H in molded body 1. Note that a hole 22 into which fixing member 12 is inserted may be provided at a position of second molding die 20 opposite fixing member 12.
[0062] Thereafter, the second molding die 20 is moved in a direction away from the first molding die 10, and the molded body 1 is removed from the first molding die 10. In this way, the molded body 1 is completed.
[0063] 5, the fixing member 12 may be moved and pulled out from the integrally molded composite material 2A and molding material 3B. This releases the fixing of the composite material 2A by the fixing member 12. That is, the method may further include a step of releasing the fixing of the composite material 2A by the fixing member 12. The fixing of the composite material 2A by the fixing member 12 may be released after step (2), before step (3), or after step (3).
[0064] If no hole 1H is formed in the molded body 1, the fixing member 12 can be moved as shown in Fig. 6 before the composite material 2A and the molding material 3B are pressed together to form an integral body. That is, the fixing of the composite material 2A by the fixing member 12 can be released after step (2) and before step (3). In this case, even if a hole 2H is formed in the composite material 2A at a position corresponding to the fixing member 12, when the composite material 2A and the molding material 3B are pressed together using the first molding die 10 and the second molding die 20 to form an integral body, the molding material 3B flows into the hole 2H, thereby filling the hole 2H.
[0065] In this way, by integrally molding the reinforcing portion 2 and the main body portion 3, a molded body 1 having excellent bonding strength between the reinforcing portion 2 and the main body portion 3 can be obtained. Furthermore, by placing a plate-shaped composite material 2A in a molding die and pressing the composite material 2A and a molding material 3B having higher fluidity than the composite material 2A, a molded body 1 having a complex shape with ribs and bosses can be manufactured.
[0066] Second Embodiment Next, a method for manufacturing a molded body according to a second embodiment will be described. Note that the same components as those in the first embodiment are designated by the same reference numerals in the last two digits, and their description will be omitted. Note that in the second embodiment, as in the first embodiment, the composite material 102A and the molding material 103B may be integrally molded by cold pressing.
[0067] 7 is a schematic cross-sectional view of a molded body 101 according to a second embodiment of the present invention, and FIGS. 8 to 13 are schematic views showing a method for manufacturing the molded body 101. In the first embodiment, molding material 3B was arranged so as to be in contact with first molding die 10, but in the second embodiment, molding material 103B is arranged so as to be in contact with second molding die 20. In other words, composite material 102A is fixed to first molding die 10 so that molding material 103B is arranged on the opposite side from first molding die 10.
[0068] The manufacturing method for producing the molded body 101 of the second embodiment includes the following steps (1) to (3): (1) a step of fixing the composite material 102A to the first molding die 10 using a plurality of fixing members 12 provided on the first molding die 10 having a cavity 11 with an area larger than that of the composite material 102A in a planar view; (2) a step of moving the second molding die 20 toward the composite material 102A fixed to the first molding die 10 and bringing the second molding die 20 into contact with the composite material 102A; and (3) a step of pressing the composite material 102A and the molding material 103B together using the first molding die 10 and the second molding die 20 to mold them into a single unit.
[0069] Specifically, first, as shown in FIG. 8 , composite material 102A is fixed in cavity 11 of first molding die 10 by a plurality of fixing members 12. Next, as shown in FIG. 9 , before step (2), molding material 103B is laminated on composite material 102A fixed to first molding die 10. Note that a step of laminating molding material 103B on composite material 102A may be included before step (1). In this case, it is preferable that in step (1), the laminate of composite material 102A and molding material 103B is fixed to first molding die 10 so that molding material 103B is positioned on the opposite side of first molding die 10. That is, in step (1), as shown in FIG. 9 , the laminate of composite material 102A and molding material 103B may be fixed in cavity 11 of first molding die 10 by a plurality of fixing members 12 so that molding material 103B is positioned on the opposite side of first molding die 10.
[0070] 10, second molding die 20 is moved toward composite material 102A fixed to first molding die 10, and second molding die 20 is brought into contact with composite material 102A. At this time, second molding die 20 may come into contact with molding material 103B layered on composite material 102A.
[0071] 11 , composite material 102A and molding material 103B are pressed together into a single piece using first molding die 10 and second molding die 20. At this time, holes 102H are formed in composite material 102A at positions corresponding to fixing member 12, and holes 103H are formed in molding material 103B at positions corresponding to fixing member 12.
[0072] Thereafter, the second molding die 20 is moved in a direction away from the first molding die 10, and the molded body 101 is removed from the first molding die 10. In this way, the molded body 101 is completed.
[0073] 12 , fixing member 12 may be moved and pulled out from integrally molded composite material 102A and molding material 103B. This releases fixing of composite material 102A by fixing member 12. That is, the method may further include a step of releasing fixing of composite material 102A by fixing member 12. Note that fixing of composite material 102A by fixing member 12 may be released after step (2), before step (3), or after step (3).
[0074] If hole 101H is not to be formed in molded body 101, fixing member 12 can be moved as shown in Fig. 13 before composite material 102A and molding material 103B are pressed together to form an integral body. That is, after step (2) and before step (3), fixing of composite material 102A by fixing member 12 can be released. In this case, even if hole 102H is formed in the position of composite material 102A corresponding to fixing member 12, when composite material 102A and molding material 103B are pressed together using first molding die 10 and second molding die 20 to form an integral body, molding material 103B flows into hole 102H, thereby filling hole 102H.
[0075] 14 to 19 are schematic diagrams showing a method for producing a molded body 201 according to a third embodiment of the present invention. Note that the same components as those in the first embodiment are designated by the same reference numerals in the last two digits, and their explanations will be omitted. In the third embodiment, an injection molding material 203B is used as a molding material with higher fluidity than the composite material. The third embodiment includes a step of injecting a molding material (injection molding material 203B) between a first molding die 210 and a second molding die 220 after step (2) and before step (3) of the first embodiment.
[0076] Specifically, the manufacturing method for manufacturing the molded body 201 of the third embodiment includes the following steps (1) to (3): (1) a step of fixing the composite material 202A to the first molding die 210 using a plurality of fixing members 212 provided on the first molding die 210 having a cavity 211 with an area larger than that of the composite material 202A in a planar view; (2) a step of moving the second molding die 220 toward the composite material 202A fixed to the first molding die 210 and bringing the second molding die 220 into contact with the composite material 202A; (3) a step of injecting the injection molding material 203B between the first molding die 210 and the second molding die 220; and (4) a step of pressing the composite material 202A and the injection molding material 203B together using the first molding die 210 and the second molding die 220 to mold them into a single piece.
[0077] The following step may be included before step (1): (0) a step of heating the composite material 202A to a first predetermined temperature, in which the first molding die 210 and the second molding die 220 are set to a second predetermined temperature.
[0078] Specifically, first, as shown in FIG. 14, a composite material 202A is fixed in a cavity 211 of a first molding die 210 by a plurality of fixing members 212.
[0079] Next, as shown in FIG. 15, the second molding die 220 is moved toward the composite material 202A fixed to the first molding die 210, and the second molding die 220 is brought into contact with the composite material 202A.
[0080] Next, as shown in FIG. 16 , injection molding material 203B is injected between first molding die 210 and composite material 202A through gate 213 provided on first molding die 210. The timing of injection of injection molding material 203B may be immediately before or immediately after pressure begins to be applied to a portion of composite material 202A from second molding die 220. To prevent misalignment of composite material 202A within the molding die, it is preferable to inject injection molding material 203B immediately after second molding die 220 contacts at least a portion of composite material 202A and begins applying pressure to composite material 202A. The method for injecting injection molding material 203B into the molding die is not particularly limited, and any conventionally known method can be used. At this time, composite material 202A is pressed against second molding die 220 by the pressure of injection molding material 203B.
[0081] Injection molding material 203B is preferably kneaded and filled between first molding die 210 and composite material 202A. By pressing injection molding material 203B after filling the mold, it is possible to prevent composite material 202A from shifting in position.
[0082] When the injection molding material 203B is poured into the mold, it is preferably heated to a temperature above the melting point and below the decomposition temperature of the thermoplastic resin if the thermoplastic resin contained in the injection molding material 203B is crystalline, or above the glass transition temperature and below the decomposition temperature of the thermoplastic resin if the thermoplastic resin is amorphous.
[0083] To fill the gap between first molding die 210 and composite material 202A with injection molding material 203B, it is sufficient to stop the descent of second molding die 220 once before the molding die is completely closed. The descent of second molding die 220 is preferably stopped after second molding die 220 comes into contact with composite material 202A. By restricting the movement of composite material 202A by having composite material 202A come into contact with second molding die 220, it is possible to prevent displacement of composite material 202A during pressing.
[0084] Next, as shown in FIG. 17 , composite material 202A and injection molding material 203B are pressed into a mold to be integrally molded. At this time, hole 202H is formed in composite material 202A at a position corresponding to fixing member 212, and hole 203H is formed in injection molding material 203B at a position corresponding to fixing member 212. In other words, fixing member 212 is a hole-forming member that forms hole 201H in molded body 201. Note that hole 222 into which fixing member 212 is inserted may be provided at a position in second mold 220 opposite fixing member 212. Thereafter, second mold 220 is moved in a direction away from first mold 210, and molded body 201 is removed from first mold 210. Thus, molded body 201 is completed.
[0085] In this way, the injection molding material 203B is injected into the mold while the composite material 202A is fixed by the fixing member 212, so even if the injection molding material 203B flows within the mold, the position of the composite material 202A can be prevented from shifting.
[0086] 18 , fixing member 212 may be moved and pulled out from integrally molded composite material 202A and injection molding material 203B. This releases composite material 202A from fixing member 212. That is, the method may further include a step of releasing composite material 202A from fixing member 212. Composite material 202A may be released from fixing member 212 after step (3), before step (4), or after step (4). After step (2) of bringing second molding die 220 into contact with composite material 202A, and before the step of releasing composite material 202A from its fixed state, the method may include a step of injecting injection molding material 203B between first molding die 210 and composite material 202A.
[0087] Furthermore, if hole 201H is not formed in molded body 201, fixing member 212 can be moved as shown in Fig. 19 before composite material 202A and injection molding material 203B are pressed together to form an integral body. That is, after step (3) and before step (4), fixing of composite material 202A by fixing member 212 can be released. In this case, even if hole 202H is formed in composite material 202A at a position corresponding to fixing member 212, injection molding material 203B flows into hole 202H when composite material 202A and injection molding material 203B are pressed together using first molding die 210 and second molding die 220 to form an integral body, thereby filling hole 202H.
[0088] 20 to 25 are schematic diagrams showing a method for manufacturing a molded product 301 according to a fourth embodiment of the present invention. The same components as those in the third embodiment are designated by the same reference numerals in the last two digits, and their explanations will be omitted. The fourth embodiment differs from the third embodiment in that an injection molding material 303B is injected between a second mold 320 and a composite material 302A.
[0089] Specifically, first, as shown in FIG. 20, a composite material 302A is fixed in a cavity 311 of a first molding die 310 by a plurality of fixing members 312.
[0090] Next, as shown in FIG. 21, the second molding die 320 is moved toward the composite material 302A fixed to the first molding die 310, and the second molding die 320 is brought into contact with the composite material 302A.
[0091] Next, as shown in FIG. 22, injection molding material 303B is injected through gate 323 provided in second molding die 320 into the space between second molding die 320 and composite material 302A.
[0092] Next, as shown in Figure 23, composite material 302A and injection molding material 303B are pressed into a mold to be integrally molded. At this time, hole 302H is formed in composite material 302A at a position corresponding to fixing member 312, and hole 303H is formed in injection molding material 303B at a position corresponding to fixing member 312. Note that hole 322 into which fixing member 312 is inserted may be provided in second molding die 320 at a position opposite fixing member 312. Thereafter, second molding die 320 is moved in a direction away from first molding die 310, and molded body 301 is removed from first molding die 310. In this manner, molded body 301 is completed.
[0093] 24, fixing member 312 may be moved and pulled out from integrally molded composite material 302A and injection molding material 303B. This releases composite material 302A from fixing member 312. That is, the method may further include a step of releasing composite material 302A from fixing member 312. Composite material 302A may be released from fixing member 312 after step (3), before step (4), or after step (4). After step (2) of bringing second molding die 320 into contact with composite material 302A and before the step of releasing composite material 302A from fixation, the method may include a step of injecting injection molding material 303B between second molding die 320 and composite material 302A.
[0094] Furthermore, if hole 301H is not formed in molded body 301, fixing member 312 can be moved as shown in FIG. 25 before composite material 302A and injection molding material 303B are pressed together to form an integral body. That is, after step (3) and before step (4), fixing of composite material 302A by fixing member 312 can be released. In this case, even if hole 302H is formed in composite material 302A at a position corresponding to fixing member 312, injection molding material 303B flows into hole 302H when composite material 302A and injection molding material 303B are pressed together using first molding die 310 and second molding die 320 to form an integral body.
[0095] In the above first to fourth embodiments, a pair of male and female molds, a first mold and a second mold, are used, and the first mold is a fixed mold and the second mold is a movable mold. However, the present invention is not limited to this. For example, the first mold may be a movable mold and the second mold may be a fixed mold.
[0096] In the above description, the first mold is the lower mold, the second mold is the upper mold, and the second mold opens and closes by moving up and down toward the first mold, but for example, the first mold may open and close by moving up and down toward the second mold. Alternatively, the first mold and the second mold may open and close by moving at least one of them horizontally.
[0097] [Opening and Closing Direction of Molds] When the first mold is a fixed mold and the second mold is a movable mold, and a molded body is produced by opening and closing the second mold by moving it horizontally toward the first mold, it is preferable to have at least two fixing members at different height positions. Figure 26 is a horizontal cross-sectional view showing a first mold 410 and a second mold 420 that are arranged to be openable and closable horizontally. In Figure 26, the first mold 410 is a fixed mold, and the second mold 420 is a movable mold. The first mold 410 has a fixing member 412 and a gate 413. The first mold 410 is provided with a plurality of fixing members 412 that fix the composite material 402A to the first mold 410. It is preferable that the plurality of fixing members 412 are at different horizontal positions. By providing multiple fixing members 412 at different horizontal positions on the first molding die 410, it is possible to prevent the composite material 412A from shifting in position relative to the first molding die 410. The fixing members 412 may be provided at different positions in the height direction. Three or more fixing members 412 may be provided at different positions in the height direction and the horizontal direction. Note that holes 422 into which the fixing members 412 are inserted may be provided at positions facing the fixing members 412 on the second molding die 420.
[0098] [Fixed mold and movable mold] Some molds may move. If the fixed mold moves, the mold that moves a relatively small distance is called the fixed mold, and the mold that moves a relatively large distance is called the movable mold.
[0099] [Pattern Cut] The composite material is preferably pattern-cut into a desired shape. Pattern cut refers to a composite material that is pre-cut into a desired shape to match the shape of the molded body. It does not refer to simple shapes such as squares or rectangles. For example, when manufacturing a box-shaped molded body 501 as shown in FIG. 27, the composite material 502A may be shaped to include margins in the area that constitutes the developed view of the box, as shown in FIG. 28. In FIG. 28, four side portions 502A2 are provided around a portion 502A1 that will become the bottom of the rectangular box, and a margin 502A3 is provided at the portion where the adjacent side portions 502A2 are joined during molding. Note that, although a margin 502A3 is provided only on one of the two adjacent side portions 502A2 in FIG. 28, a margin 502A3 may be provided on both.
[0100] When the resin contained in the composite material is a thermoplastic resin and the molding method is cold pressing, it is particularly preferable that the composite material be in a shape that has been pattern-cut and cut out. In the case of cold pressing, the resin begins to solidify the moment the molding die comes into contact with the composite material, so the fluidity during molding is lower than that of thermosetting resins. Therefore, if the composite material is cut into the desired shape in advance, it is easier to create a molded product of the desired shape. The pattern-cut shape is preferably a shape developed by computer inverse molding analysis from the three-dimensional shape of the press-molded product to be manufactured.
[0101] [Pattern Cutting and Fixing Members] Fixing members are more effective when the composite material is pattern-cut into a desired shape, the first molding die is fixed, and the second molding die is movable, and the second molding die is opened and closed by moving it horizontally to produce a molded body. Figure 29 is a front view showing a first molding die 510 in which a pattern-cut composite material 502A is fixed by fixing members 512. As shown in Figure 29, it is preferable to fix the composite material to the first molding die 510 by fixing members 512 at multiple horizontally spaced locations in a portion 502A1 that will become the bottom of a rectangular box, for example.
[0102] Figure 30 is a horizontal cross-sectional view showing a first molding die 510 and a second molding die 520 to which a composite material is fixed by fixing members. When the molding die opens and closes horizontally (left and right in Figure 30), the composite material needs to be positioned so that the plate surface faces up and down (perpendicular to the paper surface of Figure 30). In this case, when a pattern-cut composite material 502A is used, there is a possibility that the composite material 502A will sag in an unintended direction compared to composite materials with simple shapes such as squares or rectangles. Therefore, by appropriately fixing the composite material 502A to the first molding die 510 using fixing members 512, it is possible to effectively prevent the composite material 502A from sagging in an unintended direction. In Figure 29, the composite material may be pre-shaped so that the side portion 502A2 and margin 502A3, which are above the bottom portion 502A1 fixed to the first molding die 510 by the fixing member 512, do not collapse toward the second molding die 520 (see Figure 30), but collapse toward the first molding die 510 in advance.
[0103] [Injection from a fixed mold and design] Injection from a fixed mold and design will be described below. In the method for producing a molded article of the present invention, the first mold is a fixed mold, the second mold is a movable mold, the molding material is an injection molding material, and after step (2) and before step (3), the method includes a step of injecting the injection molding material between the first mold and the second mold, and the injection is preferably performed from the first mold, which is a fixed mold. Compared to injection from a movable mold, injection from a fixed mold is preferable because the equipment does not become too complicated.
[0104] 1. Formation of Design Surface When injection is performed from a fixed first mold, it is preferable that the design surface be formed by a movable second mold. This is because, while traces of the injection gate remain on the surface formed by the fixed first mold, no traces of the injection gate remain on the surface formed by the movable second mold. In this case, the design of the molded product can be improved by, for example, making the following adjustments between the composite material and the second mold. In the present invention, the layer formed between the composite material and the second mold is sometimes called a skin layer.
[0105] 2. Composite Material and Design Surface When injection is performed from a fixed first mold, it is preferable to fill the space between the second mold and the composite material with injection molding material. By filling the space between the movable second mold and the composite material with injection molding material, the fibers contained in the composite material can be hidden. A skin layer is formed by filling the space between the second mold and the composite material with injection molding material. As described below, the skin layer can be formed, for example, by wrapping the injection molding material around the outside of the composite material, by flowing the injection molding material through flow holes formed in the composite material, or by placing a resin sheet between the composite material and the second mold in advance. The thickness of the skin layer is preferably 50 μm or more and 300 μm or less, and more preferably 70 μm or more and 200 μm or less.
[0106] 2.1 Gate Position and Number To form a skin layer using injection molding material, the injection molding material should be filled so that it penetrates between the composite material and the cavity wall of the mold. In this case, the number of gates for injecting the injection molding material preferably satisfies 0 < n1 < n2. Here, n1 is the number of first gates provided in the region (XA) where the composite material is placed in a plan view of the mold cavity; and n2 is the number of second gates provided in a region other than the region (XA) where the composite material is placed in a plan view of the mold cavity.
[0107] For example, in the example shown in FIG. 31 , in the first molding die 610, two gates 613a are provided in region Y1, two gates 613b are provided in region XA, and two gates 613c are provided in region Y2. Region XA is the region where the composite material is placed, and regions Y1 and Y2 are regions other than region XA where the composite material is placed. Gate 613b is the first gate provided in region XA, and gates 613a and 613c are second gates provided in regions other than region XA. In this case, n1 = 2 and n2 = 4, and 0 < n1 < n2 is satisfied. When 0 < n1 < n2 is satisfied, the injection molding material injected from gates 613a and 613c spreads to the region where the composite material is placed, thereby promoting the injection molding material to penetrate between the composite material and the cavity wall surface of the second molding die (preferably the movable die).
[0108] 2.2 Gate Position and Discharge Rate To form a skin layer using injection molding material, the injection molding material should be filled so that it penetrates between the composite material and the cavity wall of the mold. In this case, the discharge rate from the gate for injecting the injection molding material preferably satisfies 0 < V1 < V2. Here, V1 is the discharge rate of the injection molding material from the first gate located in the region (XA) where the composite material is placed in a plan view of the mold cavity; and V2 is the discharge rate of the injection molding material from the second gate located in a region other than the region (XA) where the composite material is placed in a plan view of the mold cavity. For example, in the example shown in Figure 31, three gates 613a are located in region Y1, six gates 613b are located in region XA, and two gates 613c are located in region Y2. In this case, if the total amount of injection molding material discharged from gate 613b is V1 and the total amount of injection molding material discharged from gates 613a and 613c is V2, it is preferable that the relationship 0<V1<V2 be satisfied. When 0<V1<V2 is satisfied, the injection molding material injected from gates 613a and 613c spreads to area XA where the composite material is placed, which promotes the injection molding material entering between the composite material and the cavity wall surface of the second mold (preferably the movable mold).
[0109] 2.3 Flow Holes When the design surface is formed by the first molding die and the injection molding material is filled between the first molding die and the composite material, it is preferable to provide one or more flow holes X1 through which the injection molding material passes in the composite material, as shown in Figure 26, so that the injection molding material injected from a gate 413 of the first molding die 410 flows through the flow hole X1 and is injected between the composite material and the second molding die 420. By passing through the flow hole X1, the injection molding material injected from the first molding die 410 can enter between the composite material and the second molding die 420. In this case, it is preferable to provide a gate 413 in the area of the first molding die 410 where the composite material will be placed.
[0110] 2.4 Placement of Resin Sheet When a design surface is formed by the second mold, it is preferable to place a resin sheet between the composite material placed in the first mold and the second mold. By placing the resin sheet, it becomes easier to form a design surface on the molded body. If the resin sheet does not contain fibers, it is preferable because it has good transferability of the mirror surface of the second mold. The resin sheet may be laminated with the composite material before being placed in the first mold, or the composite material may be placed in the first mold and then the resin sheet may be laminated on the composite material.
[0111] 2.5 Texture When a design surface is formed by the second molding die, the design surface may have a texture formed by the second molding die. By transferring the mold surface of the second molding die to create a texture on the molded body, the reinforcing fibers contained in the composite material can be made less noticeable, improving the design. To make it easier for the mold surface of the second molding die to transfer the texture to the composite material, a resin-rich layer may be provided on the surface of the composite material, or a resin sheet may be placed between the second molding die and the composite material when the composite material is placed in the first molding die.
[0112] This application is based on Japanese Patent Application No. 2022-149322 filed on September 20, 2022 and Japanese Patent Application No. 2022-196925 filed on December 9, 2022, the contents of which are incorporated herein by reference.
[0113] DESCRIPTION OF SYMBOLS 1, 101, 201, 301, 501 Molded body 1H, 2H, 3H, 22, 101H, 102H, 103H, 201H, 202H, 203H, 222, 301H, 302H, 303H, 322, 422 Hole 2 Reinforcement portion 2A, 102A, 202A, 302A, 402A, 502A, 602A Composite material 3 Main body portion 3B, 103B Molding material 10, 210, 310, 410, 510, 610 First molding die 11, 211, 311 Cavity 12, 212, 312, 412, 512 Fixing member 20, 120, 220, 320, 420 Second molding die 203B, 303B Injection molding material 213, 323, 413, 613a, 613b, 613c Gate
Claims
1. A method for producing a molded body integrally molded from a composite material containing reinforcing fibers dispersed in an in-plane direction and a molding material having a higher fluidity than the composite material, comprising: A method for producing a molded body, comprising the following steps (1) to (3): (1) A process for fixing the composite material to a first molding die using a plurality of fixing members provided on the first molding die having a cavity with an area larger than that of the composite material in a planar view; (2) A process for moving a second molding die toward the composite material fixed to the first molding die and bringing the second molding die into contact with the composite material; (3) A process for pressing the composite material and the molding material using the first molding die and the second molding die to mold them into a single piece.
2. The method for producing a molded article according to claim 1 , further comprising the step of releasing the fixing of the composite material by the fixing member.
3. The method for producing a molded body according to claim 1 or 2, further comprising, prior to the step (1), a step of laminating the molding material onto the composite material.
4. The method for producing a molded body according to claim 3 , wherein in the step (1), the composite material is fixed to the first mold so that the molding material is in contact with the first mold.
5. The method for producing a molded body according to claim 1 or 2, wherein in the step (1), the composite material is fixed to the first mold so that the molding material is disposed on an opposite side to the first mold.
6. The method for producing a molded body according to claim 1 or 2, further comprising a step of laminating the molding material onto the composite material after the step (1) and before the step (2).
7. 3. The method for producing a molded body according to claim 1, further comprising the step of injecting the molding material between the first mold and the second mold after the step (2) and before the step (3).
8. 3. The method for producing a molded body according to claim 2, wherein the molding material is an injection molding material, and the method includes a step of injecting the molding material between the first mold and the second mold after the step (2) and before a step of releasing the fixation of the composite material by the fixing member.
9. The method for producing a molded article according to claim 7 , wherein the molding material is injected between the first mold and the composite material.
10. The method for producing a molded article according to claim 7 , wherein the molding material is injected between the second mold and the composite material.
11. The method for producing a molded body according to claim 1 or 2, wherein the first mold and the second mold are a pair of male and female molds.
12. The method for producing a molded article according to claim 11 , wherein the first mold is a fixed mold and the second mold is a movable mold.
13. The method for producing a molded article according to claim 11 , wherein the first mold is a lower mold and the second mold is an upper mold.
14. The method for producing a molded body according to claim 1 , wherein the fixing member is a hole forming member that forms holes in the molded body.
15. The method for producing a molded article according to claim 1 or 2, wherein the reinforcing fibers are randomly dispersed in two-dimensional directions in the in-plane direction of the composite material.
16. A method for producing the molded article according to claim 12, comprising the steps of: the molding material is an injection molding material, and the method includes a step of injecting the injection molding material between the first mold and the second mold after the step (2) and before the step (3); Injection is performed from the first mold. A method for producing a molded body.
17. A method for producing the molded article according to claim 16, comprising the steps of: a design surface is formed by the second molding die, and the injection molding material is filled between the second molding die and the composite material.
18. A method for producing the molded article according to claim 17, providing one or more flow holes in the composite material for the passage of the injection molding material; The injection molding material injected from the first mold flows through the flow holes and is injected between the first mold and the second mold. A method for producing a molded body.
19. A method for producing the molded article according to claim 18, comprising the steps of: The first mold has a first gate, which is a gate for injecting an injection molding material into the mold, in a region where the composite material is placed in a plan view. A method for producing a molded body.
20. A method for producing the molded article according to claim 16, comprising the steps of: A design surface is formed by the second molding die, and a resin sheet is disposed between the second molding die and the composite material. A method for producing a molded body.
21. A method for producing the molded article according to claim 17, The design surface has a grain shape formed by the second molding die. A method for producing a molded body.
22. The first mold is a fixed mold and the second mold is a movable mold, A method for producing a molded body by opening and closing the second mold by moving it in a horizontal direction, comprising the steps of: The method for producing a molded article according to claim 1 or 2, wherein there are at least two fixing members which are positioned at different heights.
23. The first mold is a fixed mold and the second mold is a movable mold, A method for producing a molded body by opening and closing the second mold by moving it in a horizontal direction, comprising the steps of: The method for producing a molded article according to claim 1 or 2, wherein there are at least two fixing members which are positioned at different horizontal positions.
24. The composite material has a pattern cut into it. A method for producing the molded article according to claim 1 or 2.
25. A method for producing the molded article according to claim 19, a second gate for injecting the injection molding material in a region other than the region in which the composite material is placed in a plan view of the first mold; the number n1 of the first gates and the number n2 of the second gates satisfy 0<n1<n2; A method for producing a molded body.
26. A method for producing the molded article according to claim 19, the first mold has a second gate for injecting the injection molding material in a region other than a region in which the composite material is disposed in a plan view; The discharge amount V1 of the injection molding material from the first gate and the discharge amount V2 of the injection molding material from the second gate satisfy 0<V1<V2. A method for producing a molded body.